Monodisperse latex

JP2022083422A5Inactive Publication Date: 2024-11-27XEROX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021189365
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-04-14
Filing Date
2021-11-22
Publication Date
2024-11-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Aqueous inkjet ink compositions face issues such as foaming, surface tension reduction, colloidal instability, and nozzle clogging due to high surfactant levels and broad resin particle size distribution, which compromise printing behavior and shelf life.

Method used

The formation of monodisperse latexes with small particle sizes (D (z,ave) ≤150 nm, D (v,90) <200 nm, and PDI≤0.05 is achieved through a method involving a monomer emulsion polymerization process without resin seeds, using specific monomers, reactive surfactants, and controlled polymerization conditions.

Benefits of technology

The method results in stable and printable aqueous inkjet ink compositions with improved stability, reduced nozzle clogging, and extended shelf life, enabling high-quality printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method for forming a latex, and a formed latex.SOLUTION: A method includes adding a monomer emulsion containing water, a monomer, an acidic monomer, a polyfunctional monomer, a first reactive surface active agent and a chain transfer agent, to a reactive surface active agent solution containing water, a second reactive surface active agent and an initiator at supply speed over a constant period, in which resin particles are formed in the latex by subjecting the monomer of the monomer emulsion to polymerization reaction, the reactive surface active agent solution does not contain a monomer other than the second reactive surface active agent, the reactive surface active agent solution does not contain a resin seed, and the monomer emulsion does not contain the resin seed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] (Cross-reference of related applications) This application is a continuation-in-part application of U.S. Patent Application No. 17 / 102,507, filed on 24 November 2020, the entirety of which is incorporated herein by reference. [Background technology]

[0002] The latex in aqueous inkjet ink compositions is often synthesized by emulsion polymerization or microemulsion polymerization of hydrophobic monomers in water. To reduce the size of the latex resin particles and improve colloidal stability, large amounts of surfactants, such as sodium dodecyl sulfonate (SDS), are often used. Excess surfactant in the resulting latex causes problems in the formulation of aqueous inkjet ink compositions, including foaming and reduced surface tension. Removing the excess surfactant also adds cost, complexity, and time, and leads to colloidal instability. Furthermore, the size distribution of the resin particles in the resulting latex is generally wide. Even a small number of large resin particles can induce particle sedimentation and nozzle clogging during printing of aqueous inkjet ink compositions formed from latex. [Overview of the Initiative] [Problems that the invention aims to solve]

[0003] Aqueous inkjet ink compositions generally contain water, a water-dispersible pigment, a hydrophilic solvent, and a binding resin. The binding resin may be provided by a specific latex, as described above. Latex is useful because it can form a water-permeable film to protect the colorants in the printed image from the aqueous inkjet ink composition. However, the addition of latex to aqueous inkjet ink compositions imposes a level of complexity and tends to impair printing behavior such as jet instability, jet latency, and nozzle clogging. The use of latex in aqueous inkjet ink compositions also reduces the shelf life of the composition.

[0004] This disclosure provides a method for forming monodisperse latex. Embodiments of the method involve small size and narrow size distribution (e.g., D (z、ave) ≤150nm, D (v、90) Resin particles having <200 and PDI ≤ 0.05 can be achieved. This is thought to contribute, at least in part, to greatly improved stability and print performance of aqueous inkjet ink compositions formed from latex. Monodisperse latex and aqueous inkjet ink compositions are also encompassed by this disclosure.

[0005] A method for forming latex is provided. In one embodiment, such a method comprises adding a monomer emulsion containing water, monomers, acidic monomers, polyfunctional monomers, a first reactive surfactant, and a chain transfer agent to a reactive surfactant solution containing water, a second reactive surfactant, and an initiator at a supply rate over a certain period of time, thereby causing the monomers of the monomer emulsion to undergo polymerization reactions to form resin particles in the latex. The reactive surfactant solution contains no monomers other than the second reactive surfactant, the reactive surfactant solution contains no resin seeds, and the monomer emulsion contains no resin seeds.

[0006] Latex is also provided. In embodiments, such latex comprises resin particles comprising a polymerization product containing monomers, acidic monomers, polyfunctional monomers, and a reactive surfactant, wherein the resin particles have a diameter of about 150 nm or less. (z、ave) D (v、90) , and have a PDI of approximately 0.050 or less.

[0007] Other key features and advantages of this disclosure will become apparent to those skilled in the art upon consideration of the following drawings, modes for carrying out the invention, and the appended claims. [Brief explanation of the drawing]

[0008] Hereinafter, exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings.

[0009] [Figure 1] Figure 1 shows the size distribution of monodisperse latex resin particles formed according to an exemplary embodiment of the present method.

[0010] [Figure 2] Figure 2 shows the size distribution of resin particles of another monodisperse latex formed according to an exemplary embodiment of the present method.

[0011] [Figure 3] Figure 3 shows a scanning transmission electron microscope (STEM) image of a dry monodisperse latex formed according to an exemplary embodiment of the present method. This image shows local crystallization and demonstrates the ability to form three-dimensional (3D) photonic crystals. [Modes for carrying out the invention]

[0012] monodisperse latex

[0013] In one aspect, a method of forming a monodisperse latex is provided. The latex includes resin particles synthesized from certain monomers by the method, which will be further described below. The following monomers and combinations thereof can be used (for example, the use of “(meth)” such as “(meth)acrylate” refers to both acrylate and methacrylate): styrene; alkyl (meth)acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, dodecyl acrylate, n-octyl acrylate, 2-chloroethyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; β-carboxyethyl acrylate (β-CEA), phenyl acrylate, methyl alpha chloroacrylate; butadiene; isoprene; methacrylonitrile; acrylonitrile; vinyl ethers such as vinyl methyl ether, vinyl isobutyl ether, and vinyl ethyl ether; vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate, and vinyl butyrate; vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone, and methyl isopropenyl ketone; vinylidene halides such as vinylidene chloride and chlorofluoro vinylidene; N-vinyl indole; N-vinyl pyrrolidone; methacrylate; acrylamide; methacrylamide; vinyl pyridine; vinyl pyrrolidone; vinyl-N-methyl pyridinium chloride; vinyl naphthalene; p-chloro styrene; vinyl chloride; vinyl bromide; vinyl fluoride; ethylene; propylene; butylene; and isobutylene. In an embodiment, the monomers used to form the resin particles of the latex include styrene and alkyl acrylate.

[0014] Acidic monomers, including (meth)acrylic acid monomers, sulfonic acid monomers, sulfonate monomers, and combinations thereof, can be used to form monodisperse latex resin particles. Exemplary acidic monomers include acrylic acid, methacrylic acid, ethacrylic acid, dimethylacrylic acid, maleic anhydride, maleic acid, styrene sulfonic acid, vinyl sulfonate, cyanoacrylic acid, vinyl acetic acid, allyl acetic acid, etyridine acetic acid, propyridine acetic acid, crotonic acid, fumaric acid, itaconic acid, sorbic acid, angelic acid, cinnamic acid, styrylacrylic acid, citraconic acid, glutaconic acid, aconitic acid, phenylacrylic acid, acrylooxypropionic acid, aconitic acid, phenylacrylic acid, acrylooxypropionic acid, vinylbenzoic acid, N-vinyl succinamide Examples include acetic acid, mesaconic acid, methacroylalanine, acryloylhydroxyglycine, sulfoethylmethacrylic acid, sulfopropylacrylic acid, styrenesulfonic acid, sulfoethylacrylic acid, 2-methacryloyloxymethane-1-sulfonic acid, 3-methacryloyloxypropane-1-sulfonic acid, 3-(vinyloxy)propane-1-sulfonic acid, ethylenesulfonic acid, vinyl sulfate, 4-vinylphenyl sulfate, ethylenephosphonic acid, vinyl phosphoric acid, vinylbenzoic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, and combinations thereof. These acidic monomers also include their salts, for example, salts of sulfonic acid.

[0015] In this embodiment, two different acidic monomers each have a different pK a Used to form monodisperse latex resin particles having a pK value. a The values ​​may differ from each other by at least 2 units, at least 3 units, at least 4 units, or at least 5 units. In embodiments, two different acidic monomers are present in the monomer emulsion used to form resin particles in a weight ratio ranging from 0.1 to 10. This includes the ranges of 0.5 to 8 and 1 to 6. In embodiments, the two different types of acidic monomers used to form resin particles include methacrylic acid and sulfonic acid.

[0016] Hydrophilic monomers can be used to form the resin particles of the monodisperse latex. The term "hydrophilic monomer" is distinguished from the "acidic monomer" described above. That is, the selected acid monomers may also be hydrophilic, but these terms refer to different, chemically distinct species of monomers. Hydrophilic monomers are generally monofunctional, i.e., they contain a single polymerizable group. Exemplary hydrophilic monomers include hydroxyethyl (meth)acrylate, n-hydroxyethyl (meth)acrylamide, hydroxypropyl (meth)acrylate, and hydroxypropyl (meth)acrylamide, ethylene glycol (meth)acrylate, propylene glycol (meth)acrylate, poly(ethylene glycol) (meth)acrylate having a molecular weight of 200 g / mol to 2000 g / mol, and poly(propylene glycol) (meth)acrylate having a molecular weight of 200 g / mol to 2000 g / mol, and combinations thereof. In an embodiment, the hydrophilic monomer used to form the resin particles comprises poly(propylene glycol) methacrylate.

[0017] Polyfunctional monomers can be used to form monodisperse latex resin particles, i.e., those containing two or more polymerizable groups (e.g., two, three, or four). These are useful for promoting crosslinking within the resin particles. Exemplary polyfunctional monomers include poly(ethylene glycol) di(meth)acrylates, such as difunctional monomers like poly(ethylene glycol) diacrylates having molecular weights of 200 g / mol to 2000 g / mol. These difunctional monomers may also be considered hydrophilic, as described above. Other hydrophilic bifunctional monomers include diacrylate compounds bonded to alkyl chains containing ether bonds, such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #400 diacrylate, polyethylene glycol #600 diacrylate, and dipropylene glycol diacrylate; compounds obtained by substituting the acrylate of these compounds with methacrylate; diacrylate compounds bonded to chains containing aromatic groups and ether bonds, such as polyoxyethylene (2)-2,2-bis(4-hydroxyphenyl)propane diacrylate and polyoxyethylene (4)-2,2-bis(4-hydroxyphenyl)propane diacrylate; and compounds obtained by substituting the acrylate of these compounds with methacrylate. Other exemplary bifunctional monomers include diene compounds such as isoprene and butadiene, aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene, diacrylate compounds bonded to alkyl chains such as ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, 1,10-dodecanediol diacrylate, and neopentyl glycol diacrylate, as well as compounds obtained by substituting the acrylate of these compounds with methacrylate.Polyfunctional monomers include pentaerythritol triacrylate, trimethylolmethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylate, and compounds obtained by substituting the acrylate of these compounds with methacrylate.

[0018] Reactive surfactants can be used to form monodisperse latex resin particles. Suitable reactive surfactants contain polymerizable (and therefore reactive) groups such that they are incorporated into the resin particles. Exemplary reactive surfactants include anionic ether sulfate reactive surfactants such as those in the commercially available Hitenol BC series, such as Hitenol BC10-25. Other suitable reactive surfactants include polyoxyethylene alkylphenyl ether ammonium sulfate, Hitenol BC-10, BC-20, BC-2020, BC-30; polyoxyethylene styrene-phenyl ether ammonium sulfate containing Hitenol AR-10, AR-20, AR10-25, AR-2020; nonionic polyoxyethylene alkylphenyl ethers containing Noigen RN-10, RN-20, RN-30, RN-40, RN-5065; and reactive surfactants available from Ethox containing E-sperse RX-201, RX-202, RX-203, RS-1596, RS-1616, RS-1617, RS-1618, RS-1684.

[0019] Chain transfer agents may be used to form monodisperse latex. The chain transfer agent may be a mercaptan or a thiol. Suitable chain transfer agents include n-dodecylmercaptan (NDM), n-dodecanethiol (DDT), tert-dodecylmercaptan, 1-butanethiol, 2-butanethiol, octanthiol, and combinations thereof. Carbon halides such as carbon tetrabromide, carbon tetrachloride, and combinations thereof may be used as chain transfer agents.

[0020] When forming monodisperse latex, any of the monomers listed above can be used in a monomer emulsion containing a solvent. Water is commonly used as the solvent, but water-soluble or water-miscible organic solvents (e.g., ethanol) may also be used. The types of monomers and their relative amounts may be selected to adjust the properties of the resin particles / latex. However, the following amounts have been found useful for achieving resin particles with small size and a narrow size distribution.

[0021] Acidic monomers can be used in monomer emulsions in amounts ranging from 1.5% to 15% by weight. (where weight % is (total weight of acidic monomers) / (total weight of monomers in the monomer emulsion excluding reactive surfactants) * (Refers to 100). This range includes 5% to 10% by weight. As mentioned above, different pK a Two different types of acidic monomers having a value may be used in the weight ratios described above. Hydrophilic monomers may be used in the monomer emulsion in amounts ranging from 0% to 5% by weight. (Weight percent has a similar meaning to that described for acidic monomers.) This range includes 0.1% to 5% and 1% to 5% by weight. Polyfunctional monomers, including difunctional monomers, may be used in the monomer emulsion in amounts ranging from 0.01% to 5% by weight, 0.1% to 5% by weight, or 0.1% to 1% by weight. (Weight percent has a similar meaning to that described for acidic monomers.) Other monomers (e.g., styrene, alkyl (meth)acrylates) may be present in amounts ranging from 70% to 97% by weight. (Weight percent has a similar meaning to that described for acidic monomers.) This range includes 75% to 90% by weight.

[0022] Together, the amounts of the acidic monomer, hydrophilic monomer, and polyfunctional monomer (e.g., hydrophilic polyfunctional monomer) may be present in the monomer emulsion in the range of 1.5 wt% to 12 wt%. (Here, wt% is (total weight of acidic monomer, hydrophilic monomer, and polyfunctional monomer) / (total weight of monomers in the monomer emulsion excluding the reactive surfactant) * × 100). This range includes 2 wt% to 12 wt% and 5 wt% to 10 wt%.

[0023] The reactive surfactant can be used in the monomer emulsion in an amount in the range of 1.5 wt% to 6.5 wt%. (Here, wt% is (total weight of the reactive surfactant) / (total weight of monomers in the monomer emulsion including the reactive surfactant monomer) * × 100). This range includes 1.5 wt% to 5 wt%.

[0024] The chain transfer agent may be present in the monomer emulsion and may be used in various suitable amounts, for example, 0.25 wt% to 2.5 wt%. (Here, wt% is (total weight of the chain transfer agent) / (total weight of monomers in the monomer emulsion excluding the reactive surfactant) * × 100).

[0025] In embodiments, the monomer emulsion comprises (or consists of) a solvent (e.g., water), styrene, alkyl acrylate (e.g., butyl acrylate), acidic monomer, polyfunctional monomer (e.g., difunctional monomer), reactive surfactant, and chain transfer agent. In such embodiments, one or different types of monomers may be used. Similarly, one or different types of solvents and / or one or different types of chain transfer agents may be used. In embodiments, the monomer emulsion comprises (or consists of) a solvent (e.g., water), styrene, alkyl acrylate (e.g., butyl acrylate), methacrylic acid, hydrophilic monomer (e.g., poly(propylene glycol) methacrylate), polyfunctional monomer (e.g., difunctional monomer), reactive surfactant, and chain transfer agent. In these embodiments, the monomer emulsion comprises (or consists of) a solvent (e.g., water), styrene, an alkyl acrylate (e.g., butyl acrylate), two different types of acidic monomers (e.g., methacrylic acid and sulfonic acid), a bifunctional monomer (e.g., poly(ethylene glycol) diacrylate), a reactive surfactant, and a chain transfer agent. In any of these embodiments, various amounts of monomers and chain transfer agents may be used as described above. The remainder may consist of a solvent.

[0026] In at least one embodiment, the monomer emulsion is surfactant-free (i.e., does not contain) surfactants. Here, “surfactant” refers to non-reactive, non-polymerizable anionic surfactants such as sodium dodecyl sulfate (SDS), sodium dodecylbenzenesulfonate, sodium dodecylnaphthalene sulfate; dialkylbenzenealkyl nitrates; palmitic acid; alkyldiphenyl oxide disulfonates; and branched sodium dodecylbenzenesulfonate. “Surfactant” also refers to non-reactive, non-polymerizable cationic surfactants such as alkylbenzyldimethylammonium chloride, dialkylbenzenealkylammonium chloride, lauryltrimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, cetylpyridinium bromide, trimethylbromide, quaternary polyoxyethylalkylamine halogenated salts, and dodecylbenzyltriethylammonium chloride. "Surfactants" also refer to non-reactive, non-polymerizable nonionic surfactants such as polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, and block copolymers of polyethylene oxide and polypropylene oxide. Therefore, monomer emulsions may not contain any of these surfactants (i.e., they do not contain any).

[0027] The present method for forming a monodisperse latex comprises adding one of the monomer emulsions described above to a reactive surfactant solution at a supply rate over a set period of time. The reactive surfactant solution comprises a solvent and a reactive surfactant. One of the solvents and one of the reactive surfactants described above may be used. One or different types of solvents and / or reactive surfactants may be used. The reactive surfactant in the reactive surfactant solution may be the same or different type compared to the reactive surfactant that may be present in the monomer emulsion. The reactive surfactant solution may further contain a buffer. Various buffers such as sodium bicarbonate, sodium carbonate, and ammonium hydroxide may be used. The reactive surfactant may be used in an amount ranging from 1% to 10% by weight. (where wt% is (total weight of reactive surfactant) / (total weight of reactive surfactant solution)) * (Refers to 100.) This range includes 2% by weight to 5% by weight. The buffer can be used in amounts ranging from 0.25% by weight to 2.5% by weight. (Weight % has the same meaning as described above.)

[0028] The reactive surfactant solution may contain an initiator. Alternatively, a separate initiator solution containing the initiator and one of the solvents described above may be formed and added to the reactive surfactant solution. The separate initiator solution may be added before the monomer emulsion is added. One or different types of solvents and / or initiators may be used. Examples of suitable initiators include water-soluble initiators such as ammonium persulfate (APS), sodium persulfate, and potassium persulfate, as well as organic soluble initiators containing organic peroxides and azo compounds, including Vazo peroxides such as VAZO 64 (trademark), 2-methyl-2-2'-azobispropanenitrile, and VAZO 88 (trademark), 2-2'-azobisisobutylamide anhydride, and combinations thereof.Other water-soluble initiators that can be used include azoamidine compounds, such as 2,2'-azobis(2-methyl-N-phenylpropionamidine)dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine]tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine]dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine]dihydrochloride, and 2,2'-azobis[N-(2-hydroxy-ethyl)2-methylpropion Amidine dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-( Examples include 3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and combinations thereof. The initiator may be used in an amount ranging from 0.1% to 2.5% by weight (where wt% is (total weight of initiator) / (total weight of reactive surfactant solution)). * (It refers to 100.)

[0029] In some embodiments, the reactive surfactant solution comprises (or consists of) a solvent (e.g., water), a reactive surfactant, and optionally one or more initiators and buffers. In such embodiments, one or different types of these components may be used. In any of these embodiments, the amounts of reactive surfactant, initiator, and buffer may be as described above. The remainder may consist of a solvent. In at least some embodiments, the reactive surfactant solution does not contain (i.e., does not include) any of the surfactants described above. In at least some embodiments, the reactive surfactant solution does not contain (i.e., does not include) any monomers other than the reactive surfactant monomer present in the solution.

[0030] The addition of monomer emulsions to reactive surfactant solutions can be carried out under the influence of an inert gas (e.g., nitrogen) and at high temperatures (e.g., temperatures higher than room temperature, such as in the range of 50°C to 90°C). This can be achieved by purging with an inert gas and heating the reactive surfactant solution before adding the monomer emulsion, and continuing this heating during the addition of the monomer emulsion.

[0031] As described above, the monomer emulsion is added at a supply rate over a set period of time. In the presence of an initiator, the monomers of the monomer emulsion undergo polymerization to form monodisperse latex resin particles. The supply rate is slow enough so that polymerization is carried out under "monomer-deficient" conditions. This means that the supply rate is less than or equal to the rate of polymerization, for example, the rate between styrene and acrylate monomers. Exemplary supply rates range from 1 mL / min to 10 mL / min based on a total reaction volume of 1 L. Exemplary periods include those ranging from 60 minutes to 600 minutes. Polymerization can be continued for a further period after the addition of the monomer emulsion. Exemplary additional periods range from 1 hour to 18 hours. The addition of the monomer emulsion and subsequent polymerization can be carried out under an inert gas and at high temperatures. Optionally, the formed latex can be treated by standard techniques such as solidification, dissolution, and precipitation, filtration, washing, or drying. For example, if the solvent / water is removed from the latex by drying, the dried latex still contains resin particles that can be used to form the aqueous inkjet ink compositions described below. Thus, any of the disclosed aqueous inkjet ink compositions may simply contain any of the resin particles of the disclosed latex.

[0032] It should be noted that, in at least the embodiments, this method does not involve the use of resin seeds in forming monodisperse latex resin particles. This is in contrast to existing processes that use resin seeds to initiate and stabilize polymerization. Therefore, in such embodiments, neither the monomer emulsion nor the reactive surfactant solution contains such resin seeds. The polymerization reaction that forms the resin particles does not involve such resin seeds. Similarly, in at least the embodiments, this method does not involve the use of any of the surfactants described above (other than the reactive surfactant monomer).

[0033] This method may further include forming a monomer emulsion, forming a reactive surfactant solution, and / or forming an initiator solution. Each of these may be formed by combining and mixing desired components in desired amounts.

[0034] As described above, the monodisperse latex formed by this method comprises resin particles having small size and a narrow distribution. The composition of the resin particles depends on the selection of monomers and their relative amounts, as well as the polymerization reaction between the selected monomers that produces the polymerization product described above. Therefore, a variety of compositions are encompassed based on the above description, including those based on various polymerization products containing various combinations of monomers. However, in embodiments, the resin particles comprise (or consist of) a polymerization product (e.g., copolymer) of a reactant comprising styrene, alkyl acrylate (e.g., butyl acrylate), acidic monomer, polyfunctional monomer (e.g., difunctional monomer), and a reactive surfactant. In such embodiments, one or a variety of different types of monomers may be present. In embodiments, the resin particles comprise (or consist of) a polymerization product of a reactant comprising styrene, alkyl acrylate (e.g., butyl acrylate), methacrylic acid, hydrophilic monomer (e.g., poly(propylene glycol) methacrylate), polyfunctional monomer (e.g., difunctional monomer), and a reactive surfactant. In these embodiments, the resin particles comprise (or consist of) polymerization products of a reaction mixture including styrene, alkyl acrylate (e.g., butyl acrylate), two different types of acidic monomers (e.g., methacrylic acid and sulfonic acid), a difunctional monomer (e.g., poly(ethylene glycol) diacrylate), and a reactive surfactant. In each of these embodiments, initiators may be incorporated into the beginning and end of each polymer chain in the resin particles. In each of these embodiments, the resin may be crosslinked due to the polyfunctional / difunctional monomers. In each of these embodiments, monomers may be present in the resin particles in the amounts described above.

[0035] The monodisperse latex resin particles of the present invention can be characterized by their size. The size is measured using a nanoparticle analyzer such as a Malvern Nano Zetasizer. (z、ave) It can be reported as a value. In the embodiment, D- (z、ave) This range is 150nm or less, 120nm or less, 110nm or less, 100nm or less, or 60nm to 150nm or 60nm to 100nm.

[0036] Similarly, the monodisperse latex resin particles of the present invention can be characterized by their size distribution. The size distribution may be reported as a polydispersity index (PDI) measured using a nanoparticle analyzer such as Malvern Nano-ZS. In embodiments, the PDI is ≤0.1, ≤0.050, ≤0.025, ≤0.010, ≤0.005, or in the range of 0.001 to 0.1.

[0037] Due to their small size and narrow size distribution, the monodisperse latex resin particles of the present invention can be further characterized by the absence (i.e., not containing) large particles. This includes particles smaller than 200 nm, smaller than 175 nm, or smaller than 150 nm. (v、90) It can be proven by the value.

[0038] The small size and narrow size distribution of the monodisperse latex of the present invention can be further demonstrated by its ability to form three-dimensional (3D) photonic crystals when the solvent is removed from the latex (i.e., dried). Such crystal formation is possible due to the uniform size of the resin particles. The ability to form local crystals and 3D photonic crystals can be confirmed using a scanning tunneling electron microscope (STEM). (See Figure 3.) 3D photonic crystals can be achieved using controlled heating.

[0039] Water-based inkjet ink composition

[0040] Any of the monodisperse latexes described above may be used to provide an aqueous inkjet ink composition. As described above, the small size and narrow distribution of latex resin particles are thought to contribute, at least in part, to the significantly improved stability and print performance of the aqueous inkjet ink composition. Latex may be present in the aqueous inkjet ink composition in an amount ranging from 1% to 10% by weight (where weight % is (total weight of dry latex) / (total weight of aqueous inkjet ink composition)). * (Refers to 100.) This range includes 5% to 10% by weight. Various other components can be used to form the aqueous inkjet ink compositions described below.

[0041] Solvent system

[0042] Aqueous inkjet ink compositions contain a water-based solvent system. The solvent system may consist solely of water or may include a mixture of water and a water-soluble and / or water-miscible organic solvent. Water-soluble and water-miscible organic solvents may be referred to herein as cosolvents or humectants. Suitable such organic solvents include aliphatic alcohols, aromatic alcohols, diols, glycol ethers, polyglycol ethers, long-chain alcohols, primary aliphatic alcohols, secondary aliphatic alcohols, 1,2-alcohols, 1,3-alcohols, 1,5-alcohols, ethylene glycol alkyl ethers, propylene glycol alkyl ethers, methoxylated glycerols, and ethoxylated glycerols. Exemplary examples include ethylene glycol, propylene glycol, diethylene glycol, glycerin, dipropylene glycol, trimethylolpropane, 1,2-hexanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-hydroxymethyl-1,3-propanediol, 3-methoxybutanol, 3-methyl-1,5-pentanediol, 1,3-propanediol, 1,4-butanediol, and 2,4-heptanediol.Other suitable solvents include amides, ethers, ureas, substituted ureas such as thiourea, ethyleneurea, alkylurea, alkylthiourea, dialkylurea, and dialkylthiourea, carboxylic acids and their salts such as 2-methylpentanoic acid, 2-ethyl-3-propylacrylic acid, 2-ethylhexanoic acid, 3-ethoxypropionic acid, esters, organic sulfides, organic sulfoxides, sulfones (such as sulfolanes), carbitols, butylcarbitols, cellusolve, ethers, and Examples include repropylene glycol monomethyl ether, ether derivatives, hydroxy ethers, amino alcohols, ketones, N-methylpyrrolidinone, 2-pyrrolidinone, cyclohexylpyrrolidone, amides, sulfoxides, lactones, polyelectrolytes, methylsulfonylethanol, imidazole, 1,3-dimethyl-2-imidazolidinone, betaine, sugars, such as 1-deoxy-D-galactitol, mannitol, and inositol, as well as substituted and unsubstituted formamides and substituted and unsubstituted acetamides. Combinations of these organic solvents may also be used.

[0043] Suitable water-soluble and / or water-miscible organic solvents include glycols of hydrocarbons having 4 to 7 carbon atoms. Examples of such glycols include 1,2-pentanediol; 1,2-hexanediol; 1,5-pentanediol; 1,6-hexanediol; 3-methyl-1,3-butanediol; 1,2-butanediol; 2,4-pentanediol; 1,7-heptanediol; 3-methyl-1,5-pentanediol; trimethylolpropane; ethyleneurea; 1,2,6-hexanetriol; 1,2,3-butanetriol; sorbitol; urea; diethylene glycol; 1,2,4-butanetriol; glycerol; diglycerol; triethylene glycol; polyethylene glycol 200; and polyethylene glycol 600.

[0044] In the embodiment, the solvent system includes water, a 1,2-alcohol (e.g., 1,2-hexanediol), a glycol (e.g., propylene glycol), and glycerol.

[0045] In solvent systems containing water and organic solvents, the weight ratio of water to organic solvent, as well as the types and relative amounts of different organic solvents, may be selected to achieve certain properties of the aqueous inkjet ink composition, such as desired surface tension and viscosity. In embodiments, the weight ratio of water to organic solvent is 90:10 to 51:49. If more than one organic solvent is used, these weight ratios refer to the total amount of organic solvents. Since water may be present in latex, colorants, etc., these weight ratios refer to the total amount of water.

[0046] Similarly, various total amounts of solvent systems can be used in aqueous inkjet ink compositions. In embodiments, the solvent system is present in amounts of 50% to 95% by weight, 60% to 90% by weight, or 65% to 90% by weight. (where weight % is (total weight of solvent system) / (total weight of aqueous inkjet ink composition)) * (Refers to 100.) In this embodiment, the total amount of water present is at least 50% by weight, at least 60% by weight, at least 80% by weight, or in the range of 50% to 95% by weight. (Here, weight % is (total weight of water) / (total weight of aqueous inkjet ink composition) * (It refers to 100.)

[0047] Water-soluble resin

[0048] Water-soluble resins can be used in aqueous inkjet ink compositions. The type and amount may also be selected to achieve the desired viscosity. Exemplary water-soluble resins include polyethylene glycol and polyvinylpyrrolidone. The molecular weight of the water-soluble resin may be in the range of 1,000 g / mol to 10,000 g / mol. However, it has been found that at least some embodiments of aqueous inkjet ink compositions are surprisingly susceptible to the type and molecular weight of the water-soluble resin. This finding is further described in the following examples. In the embodiments, the water-soluble resin is polyethylene glycol having molecular weights in the range of 3,000 g / mol to 9,000 g / mol, 3,000 g / mol to 7,000 g / mol, 3,000 g / mol to 5,000 g / mol, or 4,000 g / mol. These molecular weight values ​​can be determined using gel permeation chromatography. In the embodiment, the amount of water-soluble resin is selected such that the total solids content of the aqueous inkjet ink composition (generally provided by latex, water-soluble resin, and colorant) is 5% to 15% by weight, 6% to 12% by weight, or 7% to 10% by weight. (Here, weight % is (total weight of solids) / (total weight of aqueous inkjet ink composition) * (It refers to 100.)

[0049] The aqueous inkjet ink composition may further contain other binder resins, including styrene-acrylic copolymers and vinylpyrrolidone copolymers, urethane or polyurethane dispersions, and acrylic polymers such as acrylic-urethane hybrid dispersions. More specific binder resins that may be used include those available from Johnson Polymers (BASF), such as Joncryl 661, Joncryl 8003, Joncryl 8078, Joncryl 8082, Joncryl 537, Joncryl H538, Joncryl H538, and Joncryl HPD 71E. Other exemplary water-soluble resins include Rhoplex I-1955, Rhoplex I-2426D, Rhoplex I-62, Rhoplex I-98, and Rhoplex E-1691, available from Rhohm & Haas. Other examples include Lucidene 190, Lucidene 400, and Lucidene 243, available from DSM Corporation under the names NeoCryl A-1110, NeoCryl A-2092, NeoCryl A-639, NeoRad R-440, NeoRad R-441, NeoRez N-55, 972, PVP K-15, PVP K-30, PVP K-60, and PVP K-85, and Ganex P-904LC and PVP / VA W-63, available from ISPs.

[0050] Coloring agents

[0051] Water-based inkjet ink compositions may contain colorants. Colorants include pigments, dyes, and combinations thereof. Examples of suitable dyes include anionic dyes, cationic dyes, nonionic dyes, and zwitterionic dyes. Specific examples of suitable dyes include food colorants such as black No. 1, black No. 2, red No. 40, blue No. 1, and yellow No. 7, FD&C dyes, acid black dyes (No. 1, 7, 9, 24, 26, 48, 52, 58, 60, 61, 63, 92, 107, 109, 118, 119, 131, 140, 155, 156, 172, 194), and acid red dyes (No. 1, 8, 32, 35, 37, 52, 57, 92, 115, 119, 154, 249, 254, 256), Acid Blue Dye (No. 1, 7, 9, 25, 40, 45, 62, 78, 80, 92, 102, 104, 113, 117, 127, 158, 175, 183, 193, 209), Acid Yellow Dye (No. 3, 7, 17, 19, 23, 25, 29, 38, 42, 49, 59, 61, 72, 73, 114, 128, 151), Direct Black Dye (No. 4, 14, 17 , 22, 27, 38, 51, 112, 117, 154, 168), Direct Blue Dye (No. 1, 6, 8, 14, 15, 25, 71, 76, 78, 80, 86, 90, 106, 108, 123, 163, 165, 199, 226), Direct Red Dye (No. 1, 2, 16, 23, 24, 28, 39, 62, 72, 236), Direct Yellow Dye (No. 4, 11, 12, 27, 28, 33, 34, 39, 50, 58, 86, 100, Examples include reactive dyes such as 106, 107, 118, 127, 132, 142, 157), reactive red dyes (No. 4, 31, 56, 180), reactive black dye (No. 31), and reactive yellow dye (No. 37), as well as anthraquinone dyes, monoazo dyes, disazo dyes, phthalocyanine derivatives including various phthalocyanine sulfonates, aza(18)anulene, formazan copper complexes, and triphenodioxazine.

[0052] Examples of suitable pigments include black pigments, cyan pigments, magenta pigments, and yellow pigments. The pigments may be organic or inorganic particles. A suitable inorganic pigment is carbon black. However, other inorganic pigments such as cobalt blue (CoO-Al2O3), chromium yellow (PbCrO4), and iron oxide may be suitable. Suitable organic pigments include, for example, azo pigments such as diazo pigments and monoazo pigments, polycyclic pigments (e.g., phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green), perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, pyrantron pigments, and quinophthalone pigments), insoluble dye chelates (e.g., basic dye type chelates and acid dye type chelates), nitro pigments, nitroso pigments, and anthanthrone pigments such as PR168. Representative examples of phthalocyanine blue and green include copper phthalocyanine blue, copper phthalocyanine green, and their derivatives (pigment blue 15, pigment green 7, and pigment green 36). Representative examples of quinacridone include pigment orange 48, pigment orange 49, pigment red 122, pigment red 192, pigment red 202, pigment red 206, pigment red 207, pigment red 209, pigment violet 19, and pigment violet 42. Representative examples of anthraquinone include pigment red 43, pigment red 194, pigment red 177, pigment red 216, and pigment red 226. Representative examples of perylene include Pigment Red 123, Pigment Red 149, Pigment Red 179, Pigment Red 190, Pigment Red 189, and Pigment Red 224. Representative examples of thioindigoids include Pigment Red 86, Pigment Red 87, Pigment Red 88, Pigment Red 181, Pigment Red 198, Pigment Violet 36, and Pigment Violet 38.Representative examples of heterocyclic yellows include Pigment Yellow 1, Pigment Yellow 3, Pigment Yellow 12, Pigment Yellow 13, Pigment Yellow 14, Pigment Yellow 17, Pigment Yellow 65, Pigment Yellow 73, Pigment Yellow 74, Pigment Yellow 90, Pigment Yellow 110, Pigment Yellow 117, Pigment Yellow 120, Pigment Yellow 128, Pigment Yellow 138, Pigment Yellow 150, Pigment Yellow 151, Pigment Yellow 155, and Pigment Yellow 213. Such pigments are commercially available in powder or press cake form from many suppliers, including BASF Corporation, Engelhard Corporation, and Sun Chemical Corporation. Examples of usable black pigments include carbon pigments. Carbon pigments can be any commercially available carbon pigment that provides acceptable optical density and printing properties. Suitable carbon pigments for use in this system and method include, but are not limited to, carbon black, graphite, glassy carbon, charcoal, and combinations thereof. Such carbon pigments can be manufactured by various known methods, such as the channel process, contact process, furnace process, acetylene process, or thermal process, and are commercially available from such suppliers such as Cabot Corporation, Columbian Chemicals Company, Evonik, and EIDuPont de Nemours and Company.Suitable carbon black pigments include MONARCH® 1400, MONARCH® 1300, MONARCH® 1100, MONARCH® 1000, MONARCH® 900, MONARCH® 880, MONARCH® 800, MONARCH® 700, CAB-O-JET® 200, CAB-O-JET® 300, CAB-O-JET® 450, REGAL®, and BLACK. Examples of pigments include, but are not limited to, those manufactured by Cabot, such as PEARLS®, ELFTEX®, MOGUL®, and VULCAN® pigments; pigments manufactured by Columbia, such as RAVEN® 5000 and RAVEN® 3500; and pigments manufactured by Evonik, such as Color Black FW200, FW2, FW2V, FW1, FW18, FW5160, FW5170, Special Black 6, Special Black 5, Special Black 4A, Special Black 4, PRINTEX® U, PRINTEX® 140U, PRINTEX® V, and PRINTEX® 140V. Other pigments include CAB-O-JET 352K, CAB-O-JET 250C, CAB-O-JET 260M, CAB-O-JET 270Y, CAB-O-JET 465M, CAB-O-JET 470Y, and CAB-O-JET 480V (available from Cabot Corporation).

[0053] The above list of pigments includes unmodified pigment microparticles, small molecule-attached pigment microparticles, and polymer-dispersed pigment microparticles.

[0054] When forming an aqueous inkjet ink composition, the colorant may be provided as a colorant dispersion containing the colorant and a solvent (e.g., water). The colorant may also be in the form of particles, and may have an average particle size of 20 nm to 500 nm, 20 nm to 400 nm, or 30 nm to 300 nm.

[0055] Various amounts of colorants can be used in aqueous inkjet ink compositions. However, generally, the amount is selected such that the total solids content of the aqueous inkjet ink composition (generally provided by latex, water-soluble resin, and colorants) is 5% to 15% by weight, 6% to 12% by weight, or 7% to 10% by weight. (where weight % is (total weight of solids) / (total weight of aqueous inkjet ink composition)) * (It refers to 100.)

[0056] surfactant

[0057] Unlike the monodisperse latex described above, aqueous inkjet ink compositions may contain one or more surfactants. Examples of suitable surfactants include anionic surfactants (such as sodium lauryl sulfate (SLS), Dextrol OC-40, Strodex PK 90, ammonium lauryl sulfate, potassium lauryl sulfate, mireth sulfate, and sodium dioctyl sulfosuccinate series), nonionic surfactants (such as Surfynol® 104 series, Surfynol® 400 series, Dynol® 604, Dynol® 607, Dynol® 810, EnviroGem® 360, Tergitol® 15-s-7, Tergitol® 15-s-9, TMN-6, TMN-100x, and secondary alcohol ethoxylate series such as Tergitol® NP-9 and Triton® X-100), and cationic surfactants (such as Chemguard S-106A, Chemguard Examples include S-208M and Chemguard S-216M. Several fluorinated or silicone surfactants can be used, such as PolyFox™ TMPF-136A, 156A, 151N, Chemguard S-761p, S-764p, Silsurf™ A008, Siltec™ C-408, BYK 345, 346, 347, 348, and 349, and polyethersiloxane copolymer TEGO™ Wet-260, 270, and 500. Several amphoteric fluorinated surfactants, such as alkylbetaine fluorosurfactants or alkylamine oxide fluorosurfactants, such as Chemguard S-500 and Chemguard S-111, can also be used.

[0058] Various amounts of surfactant can be used in aqueous inkjet ink compositions. In embodiments, the surfactant is present in an amount ranging from 0.01% to 2% by weight. (where weight % is (total weight of surfactant) / (total weight of aqueous inkjet ink composition)) *(Refers to 100.) If two or more types of surfactants are used, these amounts refer to the total amount of surfactants.

[0059] additives

[0060] Various additives can be used in aqueous inkjet ink compositions to adjust their properties. Suitable additives include one or more of the following: biocides, fungicides, stabilizers, acids or bases, phosphates, carboxylates, sulfites, amine salts, pH adjusters such as buffers, metal ion sequestering agents such as EDTA (ethylenediaminetetraacetic acid), defoamers, and wetting agents.

[0061] Various amounts of additives can be used in aqueous inkjet ink compositions. In embodiments, additives are present in amounts ranging from 0.01% to 5% by weight (where weight % is (total weight of additives) / (total weight of aqueous inkjet ink composition)). * (Refers to 100.) If two or more types of additives are used, these amounts refer to the total amount of additives.

[0062] In at least one embodiment, the aqueous inkjet ink composition is free of coagulants, flocculants, and plasticizers. In the embodiment, the ink composition is free of any pyrrolidone-based solvent such as N-methylpyrrolidone, and is free of Texanol and Texanol isobutyrate.

[0063] Similarly, the aqueous inkjet ink compositions of the present invention may not contain any resins other than those provided by the monodisperse latex of the present invention (i.e., they may not include any other resins). A single type of monodisperse latex may be used.

[0064] In these embodiments, the aqueous inkjet ink composition comprises (or consists of) a solvent system, a monodisperse latex, a colorant, and optionally one or more water-soluble resins and additives. In these embodiments, the aqueous inkjet ink composition comprises (or consists of) a solvent system, a monodisperse latex, a colorant, a water-soluble resin, and optionally additives. In any of these embodiments, the additive may be selected from stabilizers, surfactants, defoamers, wetting agents, and biocides. In any of these embodiments, the components may be selected from any of the solvent systems, monodisperse latex, colorants, water-soluble resins, and additives disclosed herein. In any of these embodiments, the amounts of the components as described above may be used. In any of these embodiments, a single type of monodisperse latex may be used. In any of the embodiments in this paragraph, the phrase “monodisperse latex” may be replaced with “resin particles.”

[0065] Aqueous inkjet ink compositions can be formed by combining and mixing desired components in desired amounts. An exemplary method includes adding one of the disclosed monodisperse latex (or resin particles) to a colorant dispersion to form a first mixture, and adding a second mixture containing a solvent system and additives to the first mixture to form an aqueous inkjet ink composition. Mixing and / or heating may be used in the method. The aqueous inkjet ink composition may be filtered before use. Exemplary details are provided in the following examples.

[0066] Aqueous inkjet ink compositions may be used to form printed images. In embodiments, such a method includes ejecting droplets of any of the disclosed aqueous inkjet ink compositions onto a substrate to form an image thereon. Such a method may further include incorporating the ink composition into an inkjet printing apparatus. The printing apparatus may use a thermal inkjet process, in which the ink composition in the nozzle is selectively heated in an image pattern, thereby ejecting droplets of the ink composition in an image pattern. Alternatively, the printing apparatus may use an acoustic inkjet process, in which droplets of the ink composition are ejected in an image pattern by an acoustic beam. In yet another embodiment, the printing apparatus may use a piezoelectric inkjet process, in which droplets of the ink composition are ejected in an image pattern by vibration of a piezoelectric vibrating element. Any suitable substrate may be used.

[0067] The method may include: injecting ink droplets in an image pattern onto an intermediate transfer member; heating the image to partially or completely remove the solvent; and transferring the ink composition in an image pattern from the intermediate transfer member to a final recording substrate. The intermediate transfer member may be heated to a temperature higher than the temperature of the final recording sheet but lower than the temperature of the ink composition in the printing apparatus. Offset or indirect printing processes are also disclosed, for example, in U.S. Patent No. 5,389,958, the disclosure of which is fully incorporated herein by reference.

[0068] Any suitable substrate or recording sheet can be used as the final recording sheet. Examples of substrates include McCoy® Gloss #100 coated substrate, Xerox® Bold uncoated substrate, Kodak photographic paper, Sterling® Ultra Web Matte (offset coating), TrueJet® Gloss Text (inkjet coated), and McCoy® Silk (offset coating). [Examples]

[0069] The following examples are provided to further define the various types of the disclosure. These examples are for illustrative purposes only and are not intended to limit the scope of the disclosure. Unless otherwise stated, proportions and percentages are by weight. As used herein, “room temperature” refers to a temperature of about 20°C to about 25°C. Example 1

[0070] A solution was prepared by mixing 1.6 grams of reactive surfactant solution (Hitenol BC1025 from Montello), 36 grams of deionized water, and 0.4 g of NaHCO3 in a glass reactor. The reaction mixture was then purged with nitrogen for 30 minutes. The reactor was then continuously purged with nitrogen while stirring at 250 rpm. The reactor was then heated to 85°C and maintained there. Separately, 0.2 grams of ammonium persulfate initiator was dissolved in 5 grams of deionized water and added to the reactor.

[0071] Separately, a monomer emulsion was prepared in the following manner: 30 g of styrene, 5 g of butyl acrylate, 3 g of methacrylic acid, 1.5 g of polypropylene glycol methacrylate 370, 0.6 g of 1-dodecanethiol (DDT), 0.12 g of PEGDA 250, 0.8 g of Hitenol BC 1025, and 15 g of deionized water were mixed intermittently to form an emulsion. The emulsified mixture was slowly supplied to the reactor for 3 hours, and the reaction was continued for 15 hours. The resulting latex was passed through a 25 μm filter and neutralized to pH 8.0 with 0.5 M KOH solution.

[0072] The dimensions of the resin particles were analyzed using Malvern Nano-ZS. The size distribution of the obtained latex resin particles is shown in Figure 1. The peak at 101.0 nm has a width of 25.16 nm and represents 100% of the resin particle volume. Other parameters were as follows:D (v、10) =71nm, D (v、50 ) = 97nm, and D (v、90) =138nm;D (z、ave) =110nm, and PDI=0.004.

[0073] STEM images of the dried latex showed localized crystallization, demonstrating its ability to form three-dimensional (3D) photonic crystals. Example 2

[0074] A solution was prepared by mixing 1.6 grams of reactive surfactant solution (Hitenol BC1025 from Montello), 36 grams of deionized water, and 0.4 g of NaHCO3 in a glass reactor. The reaction mixture was then purged with nitrogen for 30 minutes. The reactor was then continuously purged with nitrogen while stirring at 250 rpm. The reactor was then heated to 85°C and maintained there. Separately, 0.2 grams of ammonium persulfate initiator was dissolved in 5 grams of deionized water and added to the reactor.

[0075] Separately, a monomer emulsion was prepared in the following manner: 31 g of styrene, 5 g of butyl acrylate, 3 g of methacrylic acid, 0.5 g of styrene sulfonic acid, 0.6 g of 1-dodecanethiol (DDT), 0.12 g of PEGDA 250, 0.6 g of Hitenol BC 1025, and 15 g of deionized water were mixed intermittently to form an emulsion. The emulsified mixture was slowly supplied to the reactor for 3 hours, and the reaction was continued for 15 hours. The resulting latex was passed through a 25 μm filter and neutralized to pH 8.0 with a 0.5 M KOH solution.

[0076] The dimensions of the resin particles were analyzed using Malvern Nano-ZS. The size distribution of the obtained latex resin particles is shown in Figure 2. The peak at 86.74 nm has a width of 22.49 nm and represents 100% of the resin particle volume. Other parameters were as follows:D (v、10) =61nm, D (v、50) =83nm, and D (v、90) =119nm, D (z、ave) =95nm, and PDI=0.023.

[0077] As shown in Figure 3, the STEM image of the dried latex shows localized crystallization and demonstrates the ability to form three-dimensional (3D) photonic crystals. Example 3

[0078] Aqueous inkjet ink compositions were formed using the latex from Example 2. The aqueous inkjet ink compositions shown in Table 1 below were formed using the following steps.

[0079] 1. The pigment dispersion was added to deionized water and mixed using a pitch-blade propeller at a speed of approximately 950 RPM for about 15 minutes.

[0080] 2. The latex from Example 2 was slowly added to the pigment dispersion and mixed for approximately 45 minutes (Mixture A).

[0081] 3. In a separate beaker, the water-soluble resin, co-solvent, humectant, stabilizer, surfactant, and wetting agent were mixed to form a homogeneous mixture (mixture B).

[0082] 4. Mixture B was slowly added to mixture A. Once the addition was complete, the mixer speed was set to approximately 650 RPM and the components were mixed for a further 75 minutes.

[0083] 5. Add the defoaming agent and continue mixing for another 15 minutes.

[0084] 6. After mixing, the ink composition was left at room temperature for approximately 60 minutes, and then its pH, conductivity, and surface tension were checked.

[0085] 7. The ink composition was left overnight, then filtered through a glass fiber filter (0.45 μm or 1 μm) (KST-47 filtration apparatus available from Advantec MFS, Inc.).

[0086] [Table 1]

[0087] stability

[0088] The particle size and PDI of the ink composition were measured before and after 3 days of air heating aging at 60°C using a Malvern Nano-Zetasizer. The results are shown in Table 2. (z、ave) The minimal change (approximately 4%) and no change in PDI indicate that the ink composition is extremely stable. In addition, the change in ink viscosity was minimal (less than 2%) after 3 days of air heating aging at 60°C.

[0089] [Table 2]

[0090] Printing performance

[0091] The ink composition was sprayed onto different paper substrates, including Kodak photographic paper, McCoy® gloss #100, and Xerox® Bold, using a Dimatix DMP2800 printer. The key test parameters used were as follows: liquid capacity = 4.5~4.8 ng, droplet velocity = 7 m / s, frequency = 5 kHz, voltage = 16~20 V, and printing temperature = 20°C~40°C. The printing parameter was 600 × 600 dpi. Measurements were performed using a PIAS II personal image analysis system with a digital magnifying glass. A high-resolution optical module with a field of view of approximately 3.2 mm × 2.4 mm and approximately 5 μm / pixel was used to measure dot size and diameter. The results are shown in Table 3. In addition, the ink composition passed through >25 minutes of continuous spraying and showed excellent latency.

[0092] [Table 3]

[0093] Storage life

[0094] After the ink composition was ejected, it was kept in the same printing cartridge at room temperature for 8 days. After 8 days, the ink composition was ejected again. All nozzles started ejecting without any signs of blockage. All nozzles ejected continuously for >15 minutes before the test was stopped. This experiment further demonstrates the long-term storage life and colloidal stability of the ink composition. Example 4

[0095] A series of experiments were conducted to investigate the effect of water-soluble resins in latex-free versions of aqueous inkjet ink compositions. Table 4 lists the prepared samples. Table 5 lists the tested printing parameters and results.

[0096] [Table 4]

[0097] [Table 5]

[0098] The results show that while all water-soluble resins achieve acceptable viscosity, printing performance is highly susceptible to the type and molecular weight of the water-soluble resin used. Best performance is achieved with PEG 4000.

[0099] The term “exemplary” is used herein to mean an example, case, or representation. Any embodiment or design described herein as “exemplary” is not necessarily construed as being preferable or advantageous to other embodiments or designs. Furthermore, for the purposes of this disclosure, unless otherwise specified, “a” or “an” means “one or more.”

[0100] All numerical values ​​of parameters in this disclosure are expressed using the term "approximately," meaning approximate. This includes variations inherent in the measurement of the relevant parameters, as will be understood by those skilled in the art. This also includes the exact values ​​of the disclosed numerical values ​​and the rounded values ​​of the disclosed numerical values.

[0101] The foregoing description of exemplary embodiments of the Disclosure is provided for illustrative and explanatory purposes only. It is not intended to be exhaustive or to limit the Disclosure to the exact form disclosed, and modifications and variations are possible in light of the above teachings or may be obtained from practices of the Disclosure. Embodiments are selected and described in order to illustrate the principles of the Disclosure and to enable those skilled in the art to utilize the Disclosure in various embodiments as a practical application of the Disclosure, and with various modifications suitable for the particular intended use. The scope of the Disclosure is intended to be defined by the claims and equivalents thereof appended herein.

Claims

1. 1. A method for forming a latex, comprising: adding a monomer emulsion, the monomer emulsion including water, a monomer, an acidic monomer, a multifunctional monomer, a first reactive surfactant, and a chain transfer agent, at a feed rate over a period of time to a reactive surfactant solution, the reactive surfactant solution including water, a second reactive surfactant, and an initiator, so that the monomers of the monomer emulsion undergo a polymerization reaction to form resin particles in a latex; the reactive surfactant solution is free of monomers other than the second reactive surfactant, the reactive surfactant solution is free of resin seeds, the monomer emulsion is free of resin seeds, and the feed rates are selected such that the polymerization reaction occurs under monomer starved conditions.

2. 10. The method of claim 1 , wherein the monomer emulsion comprises two different acidic monomers having pKa values ​​that differ from each other by at least about 2 units.

3. 3. The method of claim 2, wherein the two different acidic monomers are present in a weight ratio of the acidic monomer having the higher pKa to the acidic monomer having the lower pKa ranging from about 0.1 to about 10.

4. The method of claim 2 , wherein the two different acidic monomers are a methacrylic acid and a sulfonic acid monomer.

5. The method of claim 4 wherein the sulfonic acid monomer is styrene sulfonic acid.

6. 2. The method of claim 1, wherein the monomer emulsion comprises styrene, an alkyl acrylate, methacrylic acid, a sulfonic acid monomer, poly(ethylene glycol) diacrylate, an anionic ether sulfate reactive surfactant, and the chain transfer agent.

7. The method of claim 6, wherein the sulfonic acid monomer is styrene sulfonic acid.

8. 2. The method of claim 1, wherein the monomer emulsion comprises styrene, an alkyl acrylate, methacrylic acid, poly(propylene glycol) methacrylate, poly(ethylene glycol) diacrylate, an anionic ether sulfate reactive surfactant, and the chain transfer agent.

9. The method of claim 1 further comprising forming the monomer emulsion and the reactive surfactant solution.

10. 10. The method of claim 9, further comprising forming an initiator solution comprising the initiator, and adding the initiator solution to the reactive surfactant solution prior to adding the monomer emulsion.

11. 2. The method of claim 1, wherein the resin particles have a D(z,ave) of about 150 nm or less, a D(v,90) of less than about 200 nm, and a polydispersity index (PDI) of about 0.050 or less.

12. 12. The method of claim 11, wherein the resin particles have a D(z,ave) of about 120 nm or less, a D(v,90) of less than about 150 nm, and a PDI of about 0.025 or less.

13. 10. The method of claim 1, wherein the resin particles crystallize to form 3D photonic crystals upon drying of the latex.

14. A method for forming a latex, comprising the steps of: adding a monomer emulsion comprising water, a monomer, an acidic monomer, a multifunctional monomer, a first reactive surfactant, and a chain transfer agent at a feed rate over a period of time to a reactive surfactant solution comprising water, a second reactive surfactant, and an initiator, so that the monomers of the monomer emulsion undergo a polymerization reaction to form resin particles in a latex; the reactive surfactant solution does not include any monomer other than the second reactive surfactant, the reactive surfactant solution does not include any resin seeds, the monomer emulsion does not include any resin seeds; the method further comprising forming the monomer emulsion and the reactive surfactant solution; and The method further comprises forming an initiator solution comprising the initiator, and adding the initiator solution to the reactive surfactant solution prior to adding the monomer emulsion.

15. A method for forming a latex, comprising the steps of: adding a monomer emulsion comprising water, a monomer, an acidic monomer, a multifunctional monomer, a first reactive surfactant, and a chain transfer agent at a feed rate over a period of time to a reactive surfactant solution comprising water, a second reactive surfactant, and an initiator, so that the monomers of the monomer emulsion undergo a polymerization reaction to form resin particles in a latex; the reactive surfactant solution does not include any monomer other than the second reactive surfactant, the reactive surfactant solution does not include any resin seeds, the monomer emulsion does not include any resin seeds; The method of claim 1, wherein the resin particles have a D(z,ave) of about 150 nm or less, a D(v,90) of less than about 200 nm, and a polydispersity index (PDI) of about 0.050 or less.