High viscosity latex
Patent Information
- Application Number
- JP2021189561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-04-14
- Filing Date
- 2021-11-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Latices for aqueous inkjet ink compositions face issues with coagulation and agglomeration due to water-soluble resins, leading to reduced electrostatic stability and waterfastness of printed images.
A method for forming high viscosity latex using unique latex formulations and processing steps, eliminating water-soluble resins by incorporating specific monomers and surfactants, resulting in mechanically robust resin particles that form high-quality films without additional resins.
The method produces latex resin particles with high viscosity and glass transition temperature, enhancing rub/scratch resistance and waterfastness of printed images in aqueous inkjet ink compositions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] (Cross-reference of related applications) This application is a continuation-in-part application of U.S. Patent Application No. 17 / 102,725, filed on 24 November 2020, and its entirety is incorporated herein by reference. [Overview of the project] [Problems that the invention aims to solve]
[0002] The latex in aqueous inkjet ink compositions is often synthesized by emulsion polymerization or microemulsion polymerization of hydrophobic monomers in water. The latex is added to the aqueous inkjet ink composition along with water, a water-dispersible colorant, and a hydrophilic solvent. The latex resin particles act as a binder, helping to form a water-permeable polymer film that protects the printed image. However, the resin particles are generally in the form of small, rigid spheres. Other water-soluble resins are added to the ink composition to adjust its viscosity and then facilitate the formation of a thin film. However, water-soluble resins can induce the coagulation and aggregation of resin particles and inhibit their electrostatic stability. Water-soluble resins also reduce the water fastness of images printed from aqueous inkjet ink compositions.
[0003] This disclosure provides methods for forming high-viscosity latex. These methods involve specific latex formulations and specific processing steps. The methods provide high viscosity and high glass transition temperature (T gA latex having the properties of ) can be achieved. As a result, the resin particles of the latex are mechanically robust. At the same time, aqueous inkjet ink compositions containing latex readily form high-quality films without the need for any added water-soluble resins. By removing water-soluble resins, images printed from aqueous inkjet ink compositions exhibit excellent abrasion / scratch resistance and water fastness. High-viscosity latex and aqueous inkjet ink compositions made therefrom are also covered by this disclosure.
[0004] A method for forming latex is provided. In one embodiment, such a method involves adding a monomer emulsion containing water, a monomer, an acidic monomer, a hydrophilic monomer, a bifunctional monomer, a first reactive surfactant, and a chain transfer agent to a reactive surfactant solution containing water, a second reactive surfactant, and an initiator at a supply rate over a set period of time, so that the monomers of the monomer emulsion undergo polymerization to form resin particles in the latex. The reactive surfactant solution contains no monomers other than the second reactive surfactant, the reactive surfactant solution contains no resin seeds, and the monomer emulsion contains no resin seeds. The latex is characterized by a solids content of about 30% and a viscosity in the range of about 10 cP to about 100 cP when measured at room temperature.
[0005] Latex is also provided. In one embodiment, such latex comprises water and resin particles, the polymerization product of a reactant including monomers, acidic monomers, hydrophilic monomers, bifunctional monomers, and reactive surfactants, and the latex is characterized by a solids content of about 30% and a viscosity in the range of about 10 cP to about 100 cP when measured at room temperature.
[0006] Other key features and advantages of this disclosure will become apparent to those skilled in the art upon consideration of the following drawings, modes for carrying out the invention, and the appended claims. [Brief explanation of the drawing]
[0007] Hereinafter, exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings.
[0008] [Figure 1] Figure 1 shows the size distribution of resin particles of high viscosity latex formed according to an exemplary embodiment of the present method.
[0009] [Figure 2] Figure 2 shows a scanning transmission electron microscope (STEM) image of a dried high-viscosity latex formed according to an exemplary embodiment of the present method. This image shows localized crystallization and demonstrates the ability to form three-dimensional (3D) photonic crystals. [Modes for carrying out the invention]
[0010] High-viscosity latex
[0011] In one aspect, a method for forming a high viscosity latex is provided. The latex contains resin particles synthesized from certain monomers by this method, which will be further described below. The following monomers and their combinations can be used (for example, the use of "(meth)acrylate" such as "(meth)" refers to both acrylate and methacrylate): styrene; alkyl (meth)acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, dodecyl acrylate, n-octyl acrylate, 2-chloroethyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; β-carboxyethyl acrylate (β-CEA), phenyl acrylate, methyl alpha chloroacrylate; butadiene; isoprene; methacrylonitrile; acrylonitrile; vinyl ethers such as vinyl methyl ether, vinyl isobutyl ether, and vinyl ethyl ether; vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate, and vinyl butyrate; vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone, and methyl isopropenyl ketone; vinylidene halides such as vinylidene chloride and chlorofluorovinylidene; N-vinyl indole; N-vinyl pyrrolidone; methacrylate; acrylamide; methacrylamide; vinyl pyridine; vinyl pyrrolidone; vinyl-N-methyl pyridinium chloride; vinyl naphthalene; p-chlorostyrene; vinyl chloride; vinyl bromide; vinyl fluoride; ethylene; propylene; butylene; and isobutylene. In an embodiment, the monomers used to form the resin particles of the latex include styrene and alkyl acrylate.
[0012] Acidic monomers, including (meth)acrylic acid monomers, sulfonic acid monomers, sulfonate monomers, and combinations thereof, can be used to form resin particles of high viscosity latex. Exemplary acidic monomers include acrylic acid, methacrylic acid, ethacrylic acid, dimethylacrylic acid, maleic anhydride, maleic acid, styrene sulfonic acid, vinyl sulfonate, cyanoacrylic acid, vinyl acetic acid, allyl acetic acid, etyridine acetic acid, propyridine acetic acid, crotonic acid, fumaric acid, itaconic acid, sorbic acid, angelic acid, cinnamic acid, styrylacrylic acid, citraconic acid, glutaconic acid, aconitic acid, phenylacrylic acid, acryloxpropionic acid, aconitic acid, phenylacrylic acid, acryloxpropionic acid, vinylbenzoic acid, and N-vinyl succinamide. Examples include dic acid, mesaconic acid, methacroylalanine, acryloylhydroxyglycine, sulfoethylmethacrylic acid, sulfopropylacrylic acid, styrenesulfonic acid, sulfoethylacrylic acid, 2-methacryloyloxymethane-1-sulfonic acid, 3-methacryloyloxypropane-1-sulfonic acid, 3-(vinyloxy)propane-1-sulfonic acid, ethylenesulfonic acid, vinyl sulfate, 4-vinylphenyl sulfate, ethylenephosphonic acid, vinyl phosphoric acid, vinylbenzoic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, and combinations thereof. These acidic monomers also include their salts, for example, salts of sulfonic acids.
[0013] In this embodiment, two different acidic monomers each have a different pK a Used to form resin particles of high viscosity latex with a pK value of two different acidic monomers. a The values may differ from each other by at least 2 units, at least 3 units, at least 4 units, or at least 5 units. In embodiments, two different acidic monomers are present in the monomer emulsion used to form resin particles in a weight ratio ranging from 0.1 to 10. This includes the ranges of 0.5 to 8 and 1 to 6. In embodiments, the two different types of acidic monomers used to form resin particles include methacrylic acid and sulfonic acid.
[0014] Hydrophilic monomers can be used to form the resin particles of the high-viscosity latex. The term "hydrophilic monomer" is distinguished from the "acidic monomer" described above. That is, the selected acid monomers may also be hydrophilic, but these terms refer to different chemically distinct species of monomers. Hydrophilic monomers are generally monofunctional, i.e., contain a single polymerizable group. Suitable hydrophilic monomers are those that can absorb a relatively substantial amount of water via hydrogen bonds formed between the water-binding and hydrogen-bonding moieties of the hydrophilic monomer. Hydroxyl and glycol moieties are exemplary hydrogen-bonding moieties. For example, poly(ethylene glycol)- and poly(propylene glycol)-based hydrophilic monomers are particularly useful because the glycol-containing chains can absorb a substantial amount of water. Suitable hydrophilic monomers also polymerize near the surface of the resin particles such that the hydrogen-bonding moieties extend from the surface of the resin particles into the surrounding aqueous medium. Thus, the incorporation of hydrophilic monomers into the resin particles contributes to the high viscosity of the latex of the present invention.
[0015] However, it is particularly difficult to incorporate hydrophilic monomers, especially in the amounts described herein, into resin particles containing hydrophobic monomers such as styrene, alkyl (meth)acrylates. This is because, instead of copolymerizing with other desired monomers to form resin particles, hydrophilic monomers tend to undergo solution polymerization in the surrounding aqueous medium. Further, unincorporated hydrophilic monomers tend to leach out of the resin particles into the aqueous medium of the aqueous inkjet ink composition over time. The present disclosure is based on the unique latex formulations and latex processing steps disclosed herein to address these difficulties.
[0016] As described above, exemplary hydrophilic monomers include those containing a hydroxyl moiety, such as hydroxyethyl (meth)acrylate, n-hydroxyethyl (meth)acrylamide, hydroxypropyl (meth)acrylate, and hydroxypropyl (meth)acrylamide. Other exemplary hydrophilic monomers include those containing a glycol moiety, such as ethylene glycol (meth)acrylate and propylene glycol (meth)acrylate. Poly(ethylene glycol)(meth)acrylate and poly(propylene glycol)(meth)acrylate are other examples. In embodiments, the hydrophilic monomer is poly(ethylene glycol)(meth)acrylate having a molecular weight in the range of 185 g / mol to 1500 g / mol. This includes the ranges of 360 g / mol to 1500 g / mol and 500 g / mol to 1000 g / mol. In embodiments, the hydrophilic monomer is poly(propylene glycol)(meth)acrylate having a molecular weight in the range of 260 g / mol to 1000 g / mol. This includes the ranges of 360 g / mol to 1000 g / mol and 500 g / mol to 1000 g / mol. These molecular weight values can be determined using gel permeation chromatography. The types of hydrophilic monomers described herein have been found to be particularly useful in achieving the viscosities described herein while addressing the difficulties described herein.
[0017] Polyfunctional monomers can be used to form resin particles of high-viscosity latex, i.e., those containing two or more polymerizable groups (e.g., two, three, or four). These are useful for promoting crosslinking within the resin particles. Exemplary polyfunctional monomers include difunctional monomers such as poly(ethylene glycol) diacrylate, e.g., poly(ethylene glycol) diacrylate with a molecular weight of 250 g / mol. Other poly(ethylene glycol) di(meth)acrylates may be used, including those with molecular weights in the ranges of 214 g / mol to 1000 g / mol, 214 g / mol to 500 g / mol, and 214 g / mol to 300 g / mol. These molecular weight values can be determined using gel permeation chromatography. These types of difunctional monomers have been found to be particularly useful in achieving the viscosities described herein. These difunctional monomers may also be considered hydrophilic as described above. Other hydrophilic bifunctional monomers include diacrylate compounds bonded to alkyl chains containing ether bonds, such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #400 diacrylate, polyethylene glycol #600 diacrylate, and dipropylene glycol diacrylate; compounds obtained by substituting the acrylate of these compounds with methacrylate; diacrylate compounds bonded to chains containing aromatic groups and ether bonds, such as polyoxyethylene (2)-2,2-bis(4-hydroxyphenyl)propane diacrylate and polyoxyethylene (4)-2,2-bis(4-hydroxyphenyl)propane diacrylate; and compounds obtained by substituting the acrylate of these compounds with methacrylate.Other bifunctional monomers include diene compounds such as isoprene and butadiene, aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene, diacrylate compounds bonded to alkyl chains such as ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, 1,10-dodecanediol diacrylate, and neopentyl glycol diacrylate, as well as compounds obtained by substituting the acrylate of these compounds with methacrylate. Polyfunctional monomers include pentaerythritol triacrylate, trimethylolmethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylates, and compounds obtained by substituting the acrylate of these compounds with methacrylate.
[0018] Reactive surfactants can be used to form resin particles of high-viscosity latex. Suitable reactive surfactants contain polymerizable (and therefore reactive) groups that are incorporated into the resin particles. Exemplary reactive surfactants include anionic ether sulfate reactive surfactants such as those in the commercially available Hitenol BC series, such as Hitenol BC10-25. Other suitable reactive surfactants include polyoxyethylene alkylphenyl ether ammonium sulfate, Hitenol BC-10, BC-20, BC-2020, BC-30; polyoxyethylene styrene-phenyl ether ammonium sulfate containing Hitenol AR-10, AR-20, AR10-25, AR-2020; nonionic polyoxyethylene alkylphenyl ethers containing Noigen RN-10, RN-20, RN-30, RN-40, RN-5065; and reactive surfactants available from Ethox containing E-sperse RX-201, RX-202, RX-203, RS-1596, RS-1616, RS-1617, RS-1618, RS-1684.
[0019] Chain transfer agents may be used to form high-viscosity latex. The chain transfer agent may be a mercaptan or a thiol. Suitable chain transfer agents include n-dodecylmercaptan (NDM), n-dodecanethiol (DDT), tert-dodecylmercaptan, 1-butanethiol, 2-butanethiol, octanthiol, and combinations thereof. Carbon halides such as carbon tetrabromide, carbon tetrachloride, and combinations thereof may be used as chain transfer agents.
[0020] When forming high-viscosity latex, any of the monomers listed above can be used in a monomer emulsion containing a solvent. Water is commonly used as the solvent, but water-soluble or water-miscible organic solvents (e.g., ethanol) may also be included. The type of monomer and their relative amounts depend on their viscosity and glass-glass transition temperature T g The following may be selected to adjust the properties of the resin particles / latex, including the following amounts, within the range of viscosity and T disclosed herein. g It has been found to be useful in obtaining resin particles with a specific value.
[0021] Acidic monomers can be used in monomer emulsions in amounts ranging from 1.5% to 15% by weight. (where weight % is (total weight of acidic monomers) / (total weight of monomers in the monomer emulsion excluding reactive surfactants) * (Refers to 100). This range includes 5% to 10% by weight. As mentioned above, different pK aTwo different types of acidic monomers having values may be used in the weight ratios described above. The hydrophilic monomer may be used in the monomer emulsion in an amount ranging from 1% to 15% by weight. (% by weight has a similar meaning as that described for the acidic monomer.) This range includes 2% to 15% by weight, and 5% to 15% by weight. The polyfunctional monomers including the bifunctional monomer may be used in the monomer emulsion in a similar amount. However, it has been found that the stability of the aqueous inkjet ink composition is very susceptible to the amount of the polyfunctional monomer. Therefore, in an embodiment, the amount ranges from 0.01% to 0.8% by weight, 0.03% to 0.3% by weight, or 0.4% to 0.6% by weight. Other monomers (e.g., styrene, alkyl (meth)acrylate) may be present in an amount ranging from 70% to 97% by weight. (% by weight has a similar meaning as that described for the acidic monomer.) This range includes 75% to 90% by weight.
[0022] Together, the amounts of the acidic monomer, the hydrophilic monomer, and the polyfunctional monomer (e.g., hydrophilic polyfunctional monomer) may be present in the monomer emulsion in a range of 10% to 30% by weight. (Here, % by weight refers to (total weight of acidic monomer, hydrophilic monomer, and polyfunctional monomer) / (total weight of monomers in the monomer emulsion excluding the reactive surfactant) * × 100). This range includes 15% to 30% by weight, and 15% to 25% by weight. The acidic monomer and the hydrophilic polyfunctional monomer present much higher incorporation difficulties similar to those described above for the disclosed hydrophilic monomer, so their amounts are much higher than before.
[0023] The reactive surfactant may be used in the monomer emulsion in an amount ranging from 1.5% to 6.5% by weight. (Here, % by weight refers to (total weight of the reactive surfactant) / (total weight of monomers in the monomer emulsion including the reactive surfactant monomer) * × 100). This range includes 1.5% to 5% by weight.
[0024] The chain transfer agent may be present in the monomer emulsion and may be used in various suitable amounts, for example, 0.25% to 2.5% by weight. (where wt% is (total weight of chain transfer agent) / (total weight of monomers in the monomer emulsion excluding reactive surfactants) * (It refers to 100.)
[0025] In embodiments, the monomer emulsion comprises (or consists of) a solvent (e.g., water), styrene, alkyl acrylate (e.g., butyl acrylate), acidic monomer, hydrophilic monomer, polyfunctional monomer (e.g., difunctional monomer), a reactive surfactant, and a chain transfer agent. In such embodiments, one or different types of monomers may be used. Similarly, one or different types of solvents and / or one or different types of chain transfer agents may be used. In embodiments, the monomer emulsion comprises (or consists of) a solvent (e.g., water), styrene, alkyl acrylate (e.g., butyl acrylate), two different types of acidic monomers (e.g., methacrylic acid and sulfonic acid), hydrophilic monomer (e.g., poly(ethylene glycol) methacrylate), a difunctional monomer (e.g., poly(ethylene glycol) diacrylate), a reactive surfactant, and a chain transfer agent. In any of these embodiments, amounts of various monomers and chain transfer agents may be used as described above. The remainder may consist of a solvent. These particular combinations in the amounts described above have viscosity and T within the range disclosed herein. g It has been found to be particularly useful in achieving resin particles with a specific value.
[0026] In at least one embodiment, the monomer emulsion is surfactant-free (i.e., does not contain) surfactants. Here, “surfactant” refers to non-reactive, non-polymerizable anionic surfactants such as sodium dodecylsulfate (SDS), sodium dodecylbenzenesulfonate, sodium dodecylnaphthalene sulfate; dialkylbenzenealkyl nitrates; palmitic acid; alkyldiphenyl oxide disulfonates; and branched sodium dodecylbenzenesulfonate. “Surfactant” also refers to non-reactive, non-polymerizable cationic surfactants such as alkylbenzyldimethylammonium chloride, dialkylbenzenealkylammonium chloride, lauryltrimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, cetylpyridinium bromide, trimethylbromide, quaternary polyoxyethylalkylamine halogenated salts, and dodecylbenzyltriethylammonium chloride. "Surfactants" also refer to non-reactive, non-polymerizable nonionic surfactants such as polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, and block copolymers of polyethylene oxide and polypropylene oxide. Therefore, monomer emulsions may not contain any of these surfactants (i.e., they do not contain any).
[0027] The following describes the processing steps for forming a high-viscosity latex. This method involves adding one of the monomer emulsions described above to a reactive surfactant solution at a supply rate over a set period of time. The reactive surfactant solution comprises a solvent and a reactive surfactant. One of the solvents and one of the reactive surfactants described above may be used. One or different types of solvents and / or reactive surfactants may be used. The reactive surfactant in the reactive surfactant solution may be the same or different type compared to the reactive surfactant that may be present in the monomer emulsion. The reactive surfactant solution may further contain a buffer. Various buffers such as sodium bicarbonate, sodium carbonate, and ammonium hydroxide may be used. The reactive surfactant may be used in an amount ranging from 1% to 10% by weight. (where wt% is (total weight of reactive surfactant) / (total weight of reactive surfactant solution)) * (Refers to 100.) This range includes 2% by weight to 5% by weight. The buffer can be used in amounts ranging from 0.25% by weight to 2.5% by weight. (Weight % has the same meaning as described above.)
[0028] The reactive surfactant solution may contain an initiator. Alternatively, a separate initiator solution containing the initiator and one of the solvents described above may be formed and added to the reactive surfactant solution. The separate initiator solution may be added before the monomer emulsion is added. Additional amounts of the separate initiator solution may be added after the monomer emulsion is added. One or different types of solvents and / or initiators may be used. Examples of suitable initiators include water-soluble initiators such as ammonium persulfate (APS), sodium persulfate, and potassium persulfate, as well as organic soluble initiators containing organic peroxides and azo compounds, including Vazo peroxides such as VAZO 64 (trademark), 2-methyl-2-2'-azobispropanenitrile, and VAZO 88 (trademark), 2-2'-azobisisobutylamide anhydride, and combinations thereof.Other water-soluble initiators that can be used include azoamidine compounds, such as 2,2'-azobis(2-methyl-N-phenylpropionamidine)dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine]tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine]dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine]dihydrochloride, and 2,2'-azobis[N-(2-hydroxy-ethyl)2-methylpropion Amidine dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-( Examples include 3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and combinations thereof. The initiator may be used in an amount ranging from 0.1% to 2.5% by weight (where wt% is (total weight of initiator) / (total weight of reactive surfactant solution)). * (It refers to 100.)
[0029] Silica nanoparticles may be included in the reactive surfactant solution. These are particularly useful in achieving the disclosed viscosity because they can bond to the hydrogen bonding portions of hydrophilic monomers and / or water molecules. Some existing latexes for aqueous inkjet ink compositions may contain silica nanoparticles, but they are not generally included in the polymerization process as described herein. The size of the silica nanoparticles used is generally very small, for example, silica nanoparticles with an average diameter in the range of 100 nm or less, 50 nm or less, or 5 nm to 50 nm. Silica nanoparticles may be included in the reactive surfactant solution in an amount ranging from 0.5% to 5% by weight (where wt% is (total weight of silica nanoparticles) / (total weight of reactive surfactant solution)). * This refers to 100. (The total weight of silica nanoparticles refers to the solid weight, not the weight of the silica nanoparticle solution.) Commercially available silica nanoparticles that may be used include: various grades of LUDOX Colloidal Silica such as FM, SM, HS-30, HS-40, LS, TM-40, TM-50, SM-AS, AS-30, AS-40, AM, HSA, TMA, P X-30, P t-40, P W-50, CL, and CL-P, as well as various grades of Nissan Chemical Silica such as SNOWTEX ST-20L, ST-30, ST-40, ST-50, ST-OS, ST-O, ST-O-40, ST-OL, ST-C, ST-C-30, ST-CM, ST-N, STN30G, ST-N40, ST-NS, ST-XS, ST-S, ST-UP, ST-O-UP, MA-ST-UP, ST-PS-S, AMT-330S, HX-305M1, and HX-305M5.
[0030] In some embodiments, the reactive surfactant solution comprises (or consists of) a solvent (e.g., water), a reactive surfactant, and optionally one or more of an initiator, a buffer, and silica nanoparticles. In such embodiments, one or different types of these components may be used. In any of these embodiments, the amounts of reactive surfactant, initiator, buffer, and silica nanoparticles may be as described above. The remainder may consist of a solvent. In at least some embodiments, the reactive surfactant solution does not contain (i.e., does not include) any of the surfactants described above. In at least some embodiments, the reactive surfactant solution does not contain (i.e., does not include) any monomers other than the reactive surfactant monomer present in the solution.
[0031] The addition of monomer emulsions to reactive surfactant solutions can be carried out under the influence of an inert gas (e.g., nitrogen) and at high temperatures (e.g., temperatures higher than room temperature, such as in the range of 50°C to 90°C). This can be achieved by purging with an inert gas and heating the reactive surfactant solution before adding the monomer emulsion, and continuing this heating during the addition of the monomer emulsion.
[0032] As described above, the monomer emulsion is added at a supply rate over a set period of time. In the presence of an initiator, the monomers of the monomer emulsion undergo polymerization to form resin particles of high-viscosity latex. The supply rate is slow enough so that polymerization is carried out under "monomer-deficient" conditions. This means that the supply rate is less than or equal to the rate of polymerization, for example, the rate between styrene and acrylate monomers. Exemplary supply rates range from 1 mL / min to 10 mL / min based on a total reaction volume of 1 L. Exemplary periods include those ranging from 60 minutes to 600 minutes. After the addition of the monomer emulsion, polymerization can be continued for a further period with or without the addition of further initiators. Exemplary additional periods range from 1 hour to 18 hours. Both the addition of the monomer emulsion and the polymerization after addition can be carried out under an inert gas and at high temperatures. Optionally, the formed latex can be treated by standard techniques such as solidification, dissolution, precipitation, filtration, washing, or drying. For example, if the solvent / water is removed from the latex by drying, the dried latex still contains resin particles that can be used to form the aqueous inkjet ink compositions described below. Therefore, any of the disclosed aqueous inkjet ink compositions may simply contain any of the resin particles of the disclosed latex.
[0033] It should be noted that, in at least the embodiments, this method does not involve the use of resin seeds in forming resin particles of high viscosity latex. This is in contrast to existing processes that use resin seeds to initiate and stabilize polymerization. Therefore, in such embodiments, neither the monomer emulsion nor the reactive surfactant solution contains such resin seeds. The polymerization reaction that forms the resin particles also does not involve such resin seeds. Similarly, in at least the embodiments, this method does not involve the use of any of the surfactants described above (other than reactive surfactant monomers).
[0034] This method may further include forming a monomer emulsion, forming a reactive surfactant solution, and / or forming an initiator solution. Each of these may be formed by combining and mixing desired components in desired amounts.
[0035] The composition of resin particles formed using this method depends on the selection of monomers and their relative amounts, as well as the polymerization reaction between the selected monomers that produces the polymerization product described above. Therefore, a variety of compositions are encompassed based on the above description, including those based on various polymerization products of reactants containing various combinations of monomers. However, in embodiments, the resin particles contain (or consist of) polymerization products (e.g., copolymers) of reactants containing styrene, alkyl acrylates (e.g., butyl acrylate), acidic monomers, hydrophilic monomers, polyfunctional monomers (e.g., difunctional monomers), and reactive surfactants. In such embodiments, one or different types of monomers may be present. In embodiments, the resin particles contain (or consist of) polymerization products of reactants containing styrene, alkyl acrylates (e.g., butyl acrylate), two different types of acidic monomers (e.g., methacrylic acid and sulfonic acid), hydrophilic monomers (e.g., poly(ethylene glycol) methacrylate), difunctional monomers (e.g., poly(ethylene glycol) diacrylate), and reactive surfactants. In each of these embodiments, initiators may be incorporated into the start and end of each polymer chain in the resin particles. In each of these embodiments, the resin may be crosslinked due to polyfunctional / bifunctional monomers. In each of these embodiments, monomers may be present in the resin particles in the amounts described above. For example, the amounts of acidic monomers, hydrophilic monomers, and polyfunctional monomers together may be in the range of 10% to 30% by weight in the resin particles. As described above, this weight percentage is (total weight of acidic monomers, hydrophilic monomers, and polyfunctional monomers) / (total weight of monomers in the resin particles excluding reactive surfactants). * This refers to 100. As stated above, these particular combinations in the amounts described above are viscosity and T within the range disclosed herein.g It has been found to be particularly useful in achieving resin particles with a specific value.
[0036] As described above, the latex formed by this method may be characterized by its viscosity. Viscosity values may refer to specific temperatures and specific solids content, and can be measured using a Tuning fork vibratory viscometer (Cole-Parmer) or an ARES-G2 rheometer (TA instruments), as described in the following examples. In the embodiments, the viscosity at room temperature and the 30% solids content are in the range of 10 cP to 100 cP. (When used throughout this disclosure, the 30% solids content encompasses solids content within ±5% of this value.) This includes 10 cP to 80 cP, 10 cP to 40 cP, and 15 cP to 40 cP. All of these viscosities are initial viscosities and are measured relatively soon after the formation of the latex. (See Table 2 below.)
[0037] The latex formed by this method also has a T of resin particles within it. g It may also be characterized by a value. T g The values can be measured using a Differential Scanning Calorimetry (DSC) TA Instruments Discovery DSC 2500 as described in the following embodiments. In some embodiments, T g The optimal temperature range is approximately 35°C to 100°C. This includes the ranges of 35°C to 80°C and 50°C to 80°C. These values reflect the mechanical fastness of the resin particles and the printed ink. Nevertheless, as demonstrated in the following examples, the aqueous inkjet ink composition exhibits surprisingly excellent film-forming ability. This is thought to be at least partially attributable to the incorporation of hydrophilic monomers disclosed in the resin particles, as described above.
[0038] This method can also achieve resin particles with small size and a narrow size distribution. This contributes to greatly improved stability and printing performance of aqueous inkjet ink compositions containing resin particles. The size of the resin particles was measured using a nanoparticle analyzer such as the Malvern Nano Zetasizer. (z、ave) It can be reported as a value. In the embodiment, D- (z、ave) The size distribution is in the range of 150 nm or less, 140 nm or less, 130 nm or less, 100 nm or less, or 80 nm to 150 nm. The size distribution can be reported as the polydispersity index (PDI) measured using a nanoparticle analyzer such as Malvern Nano-ZS. In embodiments, the PDI is in the range of 0.1 or less, 0.050 or less, 0.040 or less, 0.035 or less, 0.030 or less, or 0.001 to 0.1.
[0039] Due to their small size and narrow size distribution, the resin particles of the high viscosity latex of the present invention can be further characterized by the absence (i.e., not containing) large particles. This includes particles smaller than 200 nm, smaller than 175 nm, or smaller than 150 nm. (v、90) It can be proven by the value.
[0040] The small size and narrow size distribution of the high-viscosity latex of the present invention can be further demonstrated by its ability to form three-dimensional (3D) photonic crystals when the solvent is removed from the latex (i.e., dried). Such crystal formation is possible due to the uniform size distribution of the resin particles. The ability of local crystallization and 3D photonic crystal formation can be confirmed using a scanning tunneling electron microscope (STEM). (See Figure 2.) 3D photonic crystals can be achieved using controlled heating.
[0041] Water-based inkjet ink composition
[0042] Using any of the high-viscosity latexes described above, an aqueous inkjet ink composition can be provided without the need to add any water-soluble resin to further adjust the viscosity. g Despite the values, the aqueous inkjet ink composition still readily forms a film. The mechanically robust resin particles then contribute to excellent friction / scratch resistance and water fastness. Latex may be present in the aqueous inkjet ink composition in an amount ranging from 1% to 10% by weight (where wt% is (total weight of dry latex) / (total weight of aqueous inkjet ink composition)). * (Refers to 100.) This range includes 5% to 10% by weight. Various other components can be used to form the aqueous inkjet ink compositions described below.
[0043] Solvent system
[0044] Aqueous inkjet ink compositions contain a water-based solvent system. The solvent system may consist solely of water or may include a mixture of water and a water-soluble and / or water-miscible organic solvent. Water-soluble and water-miscible organic solvents may be referred to herein as cosolvents or humectants. Suitable such organic solvents include aliphatic alcohols, aromatic alcohols, diols, glycol ethers, polyglycol ethers, long-chain alcohols, primary aliphatic alcohols, secondary aliphatic alcohols, 1,2-alcohols, 1,3-alcohols, 1,5-alcohols, ethylene glycol alkyl ethers, propylene glycol alkyl ethers, methoxylated glycerols, and ethoxylated glycerols. Exemplary examples include ethylene glycol, propylene glycol, diethylene glycol, glycerin, dipropylene glycol, trimethylolpropane, 1,2-hexanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-hydroxymethyl-1,3-propanediol, 3-methoxybutanol, 3-methyl-1,5-pentanediol, 1,3-propanediol, 1,4-butanediol, and 2,4-heptanediol.Other suitable solvents include amides, ethers, ureas, substituted ureas such as thiourea, ethyleneurea, alkylurea, alkylthiourea, dialkylurea, and dialkylthiourea, carboxylic acids and their salts such as 2-methylpentanoic acid, 2-ethyl-3-propylacrylic acid, 2-ethylhexanoic acid, 3-ethoxypropionic acid, esters, organic sulfides, organic sulfoxides, sulfones (such as sulfolanes), carbitols, butylcarbitols, cellusolve, ethers, and Examples include repropylene glycol monomethyl ether, ether derivatives, hydroxy ethers, amino alcohols, ketones, N-methylpyrrolidinone, 2-pyrrolidinone, cyclohexylpyrrolidone, amides, sulfoxides, lactones, polyelectrolytes, methylsulfonylethanol, imidazole, 1,3-dimethyl-2-imidazolidinone, betaine, sugars, such as 1-deoxy-D-galactitol, mannitol, and inositol, as well as substituted and unsubstituted formamides and substituted and unsubstituted acetamides. Combinations of these organic solvents may also be used.
[0045] Suitable water-soluble and / or water-miscible organic solvents include glycols of hydrocarbons having 4 to 7 carbon atoms. Examples of such glycols include 1,2-pentanediol; 1,2-hexanediol; 1,5-pentanediol; 1,6-hexanediol; 3-methyl-1,3-butanediol; 1,2-butanediol; 2,4-pentanediol; 1,7-heptanediol; 3-methyl-1,5-pentanediol; trimethylolpropane; ethyleneurea; 1,2,6-hexanetriol; 1,2,3-butanetriol; sorbitol; urea; diethylene glycol; 1,2,4-butanetriol; glycerol; diglycerol; triethylene glycol; polyethylene glycol 200; and polyethylene glycol 600.
[0046] In the embodiment, the solvent system includes water, a 1,2-alcohol (e.g., 1,2-hexanediol), a glycol (e.g., propylene glycol), and glycerol.
[0047] In solvent systems containing water and organic solvents, the weight ratio of water to organic solvent, as well as the types and relative amounts of different organic solvents, may be selected to achieve certain properties of the aqueous inkjet ink composition, such as desired surface tension and viscosity. In embodiments, the weight ratio of water to organic solvent is 90:10 to 51:49. If more than one organic solvent is used, these weight ratios refer to the total amount of organic solvents. Since water may be present in latex, colorants, etc., these weight ratios refer to the total amount of water.
[0048] Similarly, various total amounts of solvent systems can be used in aqueous inkjet ink compositions. In embodiments, the solvent system is present in amounts of 50% to 95% by weight, 60% to 90% by weight, or 65% to 90% by weight. (where weight % is (total weight of solvent system) / (total weight of aqueous inkjet ink composition)) * (Refers to 100.) In this embodiment, the total amount of water present is at least 50% by weight, at least 60% by weight, at least 80% by weight, or in the range of 50% to 95% by weight. (Here, weight % is (total weight of water) / (total weight of aqueous inkjet ink composition) * (It refers to 100.)
[0049] Coloring agents
[0050] Water-based inkjet ink compositions may contain colorants. Colorants include pigments, dyes, and combinations thereof. Examples of suitable dyes include anionic dyes, cationic dyes, nonionic dyes, and zwitterionic dyes. Specific examples of suitable dyes include food colorants such as black No. 1, black No. 2, red No. 40, blue No. 1, and yellow No. 7, FD&C dyes, acid black dyes (No. 1, 7, 9, 24, 26, 48, 52, 58, 60, 61, 63, 92, 107, 109, 118, 119, 131, 140, 155, 156, 172, 194), acid red dyes (No. 1, 8, 32, 35, 37, 52, 57, 92, 115, 119, 154, 249, 254, 256), Acid Blue Dye (No. 1, 7, 9, 25, 40, 45, 62, 78, 80, 92, 102, 104, 113, 117, 127, 158, 175, 183, 193, 209), Acid Yellow Dye (No. 3, 7, 17, 19, 23, 25, 29, 38, 42, 49, 59, 61, 72, 73, 114, 128, 151), Direct Black Dye (No. 4 , 14, 17, 22, 27, 38, 51, 112, 117, 154, 168), Direct Blue Dye (No. 1, 6, 8, 14, 15, 25, 71, 76, 78, 80, 86, 90, 106, 108, 123, 163, 165, 199, 226), Direct Red Dye (No. 1, 2, 16, 23, 24, 28, 39, 62, 72, 236), Direct Yellow Dye (No. 4, 11, 12, 27, 28, 33, 34, 39, 50, 58, 86, 1 Examples include reactive dyes such as 00, 106, 107, 118, 127, 132, 142, 157), reactive red dyes (No. 4, 31, 56, 180), reactive black dye (No. 31), and reactive yellow dye (No. 37), as well as anthraquinone dyes, monoazo dyes, disazo dyes, phthalocyanine derivatives including various phthalocyanine sulfonates, aza(18)annulene, formazan copper complexes, and triphenodioxazine.
[0051] Examples of suitable pigments include black pigment, cyan pigment, magenta pigment, and yellow pigment. The pigment may be organic or inorganic particles. A suitable inorganic pigment is carbon black. However, other inorganic pigments such as cobalt blue (CoO-Al2O3), chromium yellow (PbCrO4), and iron oxide may be suitable. Suitable organic pigments include, for example, azo pigments such as diazo pigments and monoazo pigments, polycyclic pigments (e.g., phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green), perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, pyrantron pigments, and quinophthalone pigments), insoluble dye chelates (e.g., basic dye type chelates and acid dye type chelates), nitro pigments, nitroso pigments, and anthanthrone pigments such as PR168. Representative examples of phthalocyanine blue and green include copper phthalocyanine blue, copper phthalocyanine green, and their derivatives (pigment blue 15, pigment green 7, and pigment green 36). Representative examples of quinacridone include pigment orange 48, pigment orange 49, pigment red 122, pigment red 192, pigment red 202, pigment red 206, pigment red 207, pigment red 209, pigment violet 19, and pigment violet 42. Representative examples of anthraquinone include pigment red 43, pigment red 194, pigment red 177, pigment red 216, and pigment red 226. Representative examples of perylene include Pigment Red 123, Pigment Red 149, Pigment Red 179, Pigment Red 190, Pigment Red 189, and Pigment Red 224. Representative examples of thioindigoids include Pigment Red 86, Pigment Red 87, Pigment Red 88, Pigment Red 181, Pigment Red 198, Pigment Violet 36, and Pigment Violet 38.Representative examples of heterocyclic yellows include Pigment Yellow 1, Pigment Yellow 3, Pigment Yellow 12, Pigment Yellow 13, Pigment Yellow 14, Pigment Yellow 17, Pigment Yellow 65, Pigment Yellow 73, Pigment Yellow 74, Pigment Yellow 90, Pigment Yellow 110, Pigment Yellow 117, Pigment Yellow 120, Pigment Yellow 128, Pigment Yellow 138, Pigment Yellow 150, Pigment Yellow 151, Pigment Yellow 155, and Pigment Yellow 213. Such pigments are commercially available in powder or press cake form from many suppliers, including BASF Corporation, Engelhard Corporation, and Sun Chemical Corporation. Examples of usable black pigments include carbon pigments. Carbon pigments can be any commercially available carbon pigment that provides acceptable optical density and printing properties. Suitable carbon pigments for use in this system and method include, but are not limited to, carbon black, graphite, glassy carbon, charcoal, and combinations thereof. Such carbon pigments can be manufactured by various known methods, such as the channel process, contact process, furnace process, acetylene process, or thermal process, and are commercially available from such suppliers such as Cabot Corporation, Columbian Chemicals Company, Evonik, and EIDuPont de Nemours and Company.Suitable carbon black pigments include MONARCH® 1400, MONARCH® 1300, MONARCH® 1100, MONARCH® 1000, MONARCH® 900, MONARCH® 880, MONARCH® 800, MONARCH® 700, CAB-O-JET® 200, CAB-O-JET® 300, CAB-O-JET® 450, REGAL®, and BLACK. Examples of pigments include, but are not limited to, those manufactured by Cabot, such as PEARLS®, ELFTEX®, MOGUL®, and VULCAN® pigments; pigments manufactured by Columbia, such as RAVEN® 5000 and RAVEN® 3500; and pigments manufactured by Evonik, such as Color Black FW200, FW2, FW2V, FW1, FW18, FW5160, FW5170, Special Black 6, Special Black 5, Special Black 4A, Special Black 4, PRINTEX® U, PRINTEX® 140U, PRINTEX® V, and PRINTEX® 140V. Other pigments include CAB-O-JET 352K, CAB-O-JET 250C, CAB-O-JET 260M, CAB-O-JET 270Y, CAB-O-JET 465M, CAB-O-JET 470Y, and CAB-O-JET 480V (available from Cabot Corporation).
[0052] The above list of pigments includes unmodified pigment microparticles, small molecule-attached pigment microparticles, and polymer-dispersed pigment microparticles.
[0053] When forming an aqueous inkjet ink composition, the colorant may be provided as a colorant dispersion containing the colorant and a solvent (e.g., water). The colorant may also be in the form of particles, and may have an average particle size of 20 nm to 500 nm, 20 nm to 400 nm, or 30 nm to 300 nm.
[0054] Various amounts of colorants can be used in aqueous inkjet ink compositions. However, generally, the amount is selected such that the total solids content of the aqueous inkjet ink composition (generally provided by latex, colorants, and wax, if present) is 5% to 15% by weight, 6% to 12% by weight, or 7% to 10% by weight. (where weight % is (total weight of solids) / (total weight of aqueous inkjet ink composition)) * (It refers to 100.)
[0055] wax
[0056] Water-based inkjet ink compositions may contain wax. The type and amount may be selected to optimize the friction resistance and water fastness of the water-based inkjet ink composition. Exemplary waxes include paraffin wax, polyethylene wax, polypropylene wax, microcrystalline wax, polyolefin wax, montan ester wax, and carnauba wax. Waxes having a melting point in the range of 50°C to 150°C may be used. Michelman (e.g., Michem Lube 103DI, 124, 124P, 135, 156, 180, 182, 190, 270R, 368, 511, 693, 723, 743, 743P, and 985, and Michem) Nanoscale wax emulsions (e.g., diameters of 1000 nm or less, 500 nm or less, or 100 nm or less) based on carnauba wax and paraffin wax may be used, including those from Emulsion24414, 34935, 36840, 41740, 43040, 43240, 44730, 47950, 48040M2, 61355, 62330, 66035, 67235, 70750, 71150, 71152, 91735, 93235, 93335, 93935, and 94340. Aquacer 2500, Aquacer 507, Aquacer 513, Aquacer 530, Aquacer 531, Aquacer 532, Aquacer 535, Aquacer 537, Aquacer Waxes from Byk, including 539 and Aquacer 593, may also be used.
[0057] Nanoscale wax emulsions based on charged waxes (e.g., anionic waxes) have been found to be particularly useful in achieving desired dry and wet friction resistances (see Example 6). An exemplary such wax is Michem Lube 190.
[0058] Various amounts of wax can be used in aqueous inkjet ink compositions. However, generally, the amount is selected such that the total solids content of the aqueous inkjet ink composition is 5% to 15% by weight, 6% to 12% by weight, or 7% to 10% by weight. (where weight % is (total weight of solids) / (total weight of aqueous inkjet ink composition)) * (It refers to 100.)
[0059] surfactants
[0060] Unlike the high-viscosity latex described above, the aqueous inkjet ink composition may contain one or more surfactants. Examples of suitable surfactants include anionic surfactants (such as sodium lauryl sulfate (SLS), Dextrol OC-40, Strodex PK 90, ammonium lauryl sulfate, potassium lauryl sulfate, mireth sulfate, and sodium dioctyl sulfosuccinate series), nonionic surfactants (such as Surfynol® 104 series, Surfynol® 400 series, Dynol® 604, Dynol® 607, Dynol® 810, EnviroGem® 360, Tergitol® 15-s-7, Tergitol® 15-s-9, TMN-6, TMN-100x, and secondary alcohol ethoxylate series such as Tergitol® NP-9 and Triton® X-100), and cationic surfactants (such as Chemguard S-106A, Chemguard Examples include S-208M and Chemguard S-216M. Several fluorinated or silicone surfactants can be used, such as PolyFox™ TMPF-136A, 156A, 151N, Chemguard S-761p, S-764p, Silsurf™ A008, Siltec™ C-408, BYK 345, 346, 347, 348, and 349, and polyethersiloxane copolymer TEGO™ Wet-260, 270, and 500. Several amphoteric fluorinated surfactants, such as alkylbetaine fluorosurfactants or alkylamine oxide fluorosurfactants, such as Chemguard S-500 and Chemguard S-111, can also be used.
[0061] Various amounts of surfactant can be used in aqueous inkjet ink compositions. In embodiments, the surfactant is present in an amount ranging from 0.01% to 2% by weight. (where weight % is (total weight of surfactant) / (total weight of aqueous inkjet ink composition)) *(This refers to 100.) When two or more types of surfactants are used, these amounts refer to the total amount of surfactants.
[0062] additives
[0063] Various additives can be used in aqueous inkjet ink compositions to adjust their properties. Suitable additives include one or more of the following: biocides, fungicides, stabilizers, acids or bases, phosphates, carboxylates, sulfites, amine salts, pH adjusters such as buffers, metal ion sequestering agents such as EDTA (ethylenediamine tetraacetic acid), defoamers, and wetting agents.
[0064] Various amounts of additives can be used in aqueous inkjet ink compositions. In embodiments, additives are present in amounts ranging from 0.01% to 5% by weight (where weight % is (total weight of additives) / (total weight of aqueous inkjet ink composition)). * (This refers to 100.) If two or more additives are used, these amounts refer to the total amount of additives.
[0065] In at least one embodiment, the aqueous inkjet ink composition is free of coagulants, flocculants, and plasticizers. In the embodiment, the ink composition is free of any pyrrolidone-based solvent such as N-methylpyrrolidone, and is free of Texanol and Texanol isobutyrate.
[0066] As described above, the aqueous inkjet ink composition of the present invention does not contain (i.e., does not include) water-soluble resins. This means that it does not contain (i.e., does not include) water-soluble resins such as polyethylene glycol and polyvinylpyrrolidone. The aqueous inkjet ink composition may not contain (i.e., does not include) binder resins such as styrene-acrylic copolymers and vinylpyrrolidone copolymers, urethane or polyurethane dispersions, and acrylic polymers such as acrylic-urethane hybrid dispersions. More specific binder resins that may be excluded include those available from Johnson Polymers (BASF), such as Joncryl 661, Joncryl 8003, Joncryl 8078, Joncryl 8082, Joncryl 537, Joncryl H538, Joncryl H538, and Joncryl HPD 71E. Other exemplary water-soluble resins that are excluded include Rhoplex I-1955, Rhoplex I-2426D, Rhoplex I-62, Rhoplex I-98, and Rhoplex E-1691, available from Rhohm & Haas. Other excluded resins include Lucidene 190, Lucidene 400, and Lucidene 243, available from DSM Corporation; NeoCryl A-1110, NeoCryl A-2092, NeoCryl A-639, NeoRad R-440, NeoRad R-441, NeoRez N-55, 972, PVP K-15, PVP K-30, PVP K-60, and PVP K-85, available from ISP; and Ganex P-904LC and PVP / VA W-63.
[0067] Similarly, the aqueous inkjet ink composition of the present invention may not contain any resins other than those provided by the high-viscosity latex of the present invention (i.e., it may not include any other resins). A single type of high-viscosity latex may be used.
[0068] In the embodiments, the aqueous inkjet ink composition comprises (or consists of) a solvent system, a high-viscosity latex, a colorant, and optionally one or more waxes and additives. In the embodiments, the aqueous inkjet ink composition comprises (or consists of) a solvent system, a high-viscosity latex, a colorant, a wax, and optionally additives. In any of these embodiments, the additive may be selected from stabilizers, surfactants, defoamers, wetting agents, and biocides. In any of these embodiments, the components may be selected from any of the solvent systems, high-viscosity latex, colorants, waxes, and additives disclosed herein. In any of these embodiments, the amounts of the components as described above may be used. In any of these embodiments, a single type of high-viscosity latex may be used. In any of the embodiments in this paragraph, the phrase “high-viscosity latex” may be replaced with “resin particles.”
[0069] Aqueous inkjet ink compositions can be formed by combining and mixing desired components in desired amounts. An exemplary method includes adding one of the disclosed high-viscosity latex (or resin particles) to a colorant dispersion to form a first mixture, and adding a second mixture containing a solvent system and additives to the first mixture to form an aqueous inkjet ink composition. A third mixture containing wax may be added to the combined first and second mixtures. Mixing and / or heating may be used in the method. The aqueous inkjet ink composition may be filtered before use. Exemplary details are provided in the following examples.
[0070] Aqueous inkjet ink compositions may be used to form printed images. In embodiments, such a method includes ejecting droplets of any of the disclosed aqueous inkjet ink compositions onto a substrate to form an image thereon. Such a method may further include incorporating the ink composition into an inkjet printing apparatus. The printing apparatus may use a thermal inkjet process, in which the ink composition in the nozzle is selectively heated in an image pattern, thereby ejecting droplets of the ink composition in an image pattern. Alternatively, the printing apparatus may use an acoustic inkjet process, in which droplets of the ink composition are ejected in an image pattern by an acoustic beam. In yet another embodiment, the printing apparatus may use a piezoelectric inkjet process, in which droplets of the ink composition are ejected in an image pattern by vibration of a piezoelectric vibrating element. Any suitable substrate may be used.
[0071] The method may include: injecting ink droplets in an image pattern onto an intermediate transfer member; heating the image to partially or completely remove the solvent; and transferring the ink composition in an image pattern from the intermediate transfer member to a final recording substrate. The intermediate transfer member may be heated to a temperature higher than the temperature of the final recording sheet but lower than the temperature of the ink composition in the printing apparatus. Offset or indirect printing processes are also disclosed, for example, in U.S. Patent No. 5,389,958, the disclosure of which is fully incorporated herein by reference.
[0072] Any suitable substrate or recording sheet can be used as the final recording sheet. Examples of substrates include McCoy® Gloss #100 coated substrate, Xerox® Bold uncoated substrate, Kodak photographic paper, Sterling® Ultra Web Matte (offset coating), TrueJet® Gloss Text (inkjet coated), and McCoy® Silk (offset coating). [Examples]
[0073] The following examples are provided to further define the various types of the disclosure. These examples are for illustrative purposes only and are not intended to limit the scope of the disclosure. Unless otherwise stated, proportions and percentages are by weight. As used herein, “room temperature” refers to a temperature of about 20°C to about 25°C. Example 1
[0074] A solution was prepared by mixing 1.5 g of reactive surfactant solution (Hitenol BC 1025 from Montello), 36 g of deionized water, 0.3 g of sodium bicarbonate, and 0.7 g of silica nanoparticle solution (34% Ludox) in a glass reactor. The reaction mixture was then purged with nitrogen for 30 minutes. The reactor was then continuously purged with nitrogen while stirring at 250 rpm. The reactor was then heated to 75°C and maintained there. Separately, 0.4 g of ammonium persulfate (APS) initiator was dissolved in 5 g of deionized water and added to the reactor.
[0075] Separately, a monomer emulsion was prepared in the following manner: 28 g of styrene, 6 g of butyl acrylate, 3 g of methacrylic acid, 1 g of sodium 4-styrenesulfonate (styrenesulfonic acid), 1 g of hydroxyethyl acrylate (HEA), 0.6 g of 1-dodecanethiol (DDT), 0.2 g of PEGDA 250, 0.8 g of Hitenol BC 1025, and 16 g of deionized water were mixed to form an emulsion. The emulsified mixture was slowly supplied to the reactor for 2 hours, and the reaction was continued for 1.5 hours. A further 0.1 g of APS initiator was dissolved in deionized water and added to the reactor over 10 minutes, and the reaction was continued for another 1.5 hours. The resulting latex was cooled to room temperature and neutralized to pH 8.0 with 0.5 M KOH solution.
[0076] The latex formulations are shown in Table 1, and the latex properties are shown in Table 2. The dimensions of the latex resin particles were analyzed using Malvern Nano-ZS. The size distribution of the resin particles is shown in Figure 1. The peak at 80 nm has a width of 21 nm and represents 100% of the resin particle volume. Other parameters were as follows: D- (z、ave) =89nm, D (v、10) =55, D (v、50) =76, and D (v、90) =112, and PDI = 0.031. Monomer conversion was measured and showed a conversion rate exceeding 99.9%. Therefore, the weight of monomers in the monomer emulsion is the same as that of the resin particles, excluding the polymerizable surfactant, from calculations.
[0077] As shown in Figure 2, the STEM image of the dry latex shows localized crystallization and the ability to form three-dimensional (3D) photonic crystals. Table 2 also shows the measured viscosity and T of the latex. g Includes room temperature and 40-400s -1 To measure viscosity, a tuning fork vibratory viscometer (Cole-Parmer) or an ARES-G2 rheometer (TA instruments) was used. g The temperature was measured using a TA Instruments Discovery DSC 2500 at a rate of 10°C / min in three consecutive heating-cooling-heating cycles. g Regarding the value, this value is related to the latex resin particles. Examples 2-4
[0078] In Examples 2 and 3, the procedure of Example 1 was repeated, but hydroxyethyl acrylate was replaced with various amounts of either PEGMA 500 (having 9 ethylene glycol repeating units) or PEGMA 950 (having 19 ethylene glycol repeating units). Furthermore, silica nanoparticles were not used in Examples 2 and 3. The latex formulations are shown in Table 1, and the latex properties are shown in Table 2. Example 5 (Comparison)
[0079] In Example 5, the procedure of Example 1 was repeated, but hydrophilic monomers or silica nanoparticles were not used. The latex formulation is shown in Table 1, and the properties of the latex are shown in Table 2.
[0080] [Table 1]
[0081] [Table 2]
[0082] The results shown in Table 2 demonstrate a significant difference in viscosity between latex synthesized using hydrophilic monomers (Examples 1-4) and silica nanoparticles (Examples 1 and 4) and comparative example 5 (rigid latex with only acid functionality). The results for Examples 1-4 further demonstrate that viscosity can be controlled over a wide range. These also show that the higher the amount of hydrogen bonding in the latex, the higher the viscosity. Stability measurements (not shown) were also performed for Example 1. The room temperature viscosity of the latex measured after approximately 40 days (e.g., ±12 hours) was the same as the room temperature viscosity measured on day 1 (i.e., the initial viscosity shown in Table 2), indicating excellent incorporation of the hydrophilic monomer and no leaching. Similarly, the room temperature viscosity of the latex measured after approximately 3 days (e.g., ±12 hours) in an oven at approximately 60°C (e.g., ±5°C) was the same as the room temperature viscosity on day 1, again demonstrating excellent stability. "Same" means within ±1%.
[0083] The results shown in Table 2 also indicate that latex synthesized from hydrophilic monomers (Examples 1-4) and silica nanoparticles (Examples 1 and 4) exhibit relatively high T in their natural state (unneutralized). g This indicates that it has a value. (For example, in inkjet ink compositions, at a basic pH of 8-9, the presence of a counterion (i.e., potassium) causes the latex to have a higher T g It will have a value. ) High T gThe value indicates that the resin particles are mechanically robust, protecting images formed from the aqueous inkjet ink composition from weathering and damage. The dry and wet friction resistance of films formed from latex-containing aqueous inkjet ink compositions is further described in Example 6 below. Example 6
[0084] Aqueous inkjet ink compositions were formed using the latex from Examples 1 and 4, and Comparative Example 5. The aqueous inkjet ink compositions were formed using the following steps, and the formulations are shown in Table 3.
[0085] 1. The pigment dispersion was added to deionized water and mixed using a pitch-blade propeller at a speed of approximately 300 RPM for about 15 minutes.
[0086] 2. The latex was slowly added to the pigment dispersion, followed by the defoamer, and mixed for about 20 minutes (Mixture A).
[0087] 3. In a separate beaker, the co-solvent, humectant, stabilizer, surfactant, and wetting agent were mixed to form a homogeneous mixture (mixture B).
[0088] 4. Mixture B was slowly added to mixture A. Once the addition was complete, the components were mixed for a further 20 minutes.
[0089] 5. Add the wax and continue mixing for another 15 minutes.
[0090] 6. After mixing, the aqueous inkjet ink composition was left at room temperature for approximately 60 minutes, and then its pH, conductivity, and surface tension were checked.
[0091] [Table 3]
[0092] viscosity
[0093] Viscosity measurements showed that high-viscosity latex (Examples 1 and 4) could raise the viscosity of aqueous inkjet ink compositions to a level useful for inkjet printing (9–10 cP at 23°C) without the need for any water-soluble resins. The room-temperature viscosity of the aqueous inkjet ink composition prepared using the latex of Example 1, measured after approximately 40 days (e.g., ±12 hours), was the same as the room-temperature viscosity measured on day 1 (i.e., the initial viscosity shown in Table 3). The room-temperature viscosity of the aqueous inkjet ink composition was also measured after approximately 3 days (e.g., ±12 hours) in an oven at approximately 60°C (e.g., ±5°C). The viscosity was the same as the room-temperature viscosity measured on day 1, demonstrating excellent stability. "Same" means within ±1%.
[0094] Dry and wet friction resistance
[0095] Water-based inkjet ink compositions were tested for dry friction resistance (30 double-rubs using a dry cotton swab) and wet friction resistance (20 double-rubs using a wet cotton swab) (water fastness). A thin layer of each inkjet ink composition (wire-wound rod RDS2.5) was coated onto McCoy gloss #100 paper and then dried in a convection oven at 130°C for 2 minutes. Both wet and dry friction resistance were significantly higher for the inkjet ink compositions made using latex in Examples 1 and 4 than for those made using the latex and commercially available inkjet ink composition in Comparative Example 5.
[0096] Aqueous inkjet ink compositions similar to those shown in Table 3 were used, but further experiments were conducted by replacing Michem Lube 190 wax (a nano-sized anionic wax emulsion) with other types of wax that are not nano-sized anionic wax emulsions. Compared to these other waxes, Michem Lube 190 wax provided superior dry and wet friction resistance. Aqueous inkjet ink compositions prepared using this wax also passed the tape test, while others did not. In the tape test, one Scotch tape was fully pressed and adhered to the surface of the dried ink, left for 20 seconds, and then the tape was quickly peeled off. Passing the test was indicated by no ink transfer to the tape. Failing the test was indicated by some or all of the ink transfer to the tape.
[0097] Printing performance
[0098] Inkjet ink compositions were sprayed onto different paper substrates, including Kodak photo paper, McCoy® gloss #100, and Xerox® Bold, using a Dimatix DMP2800 printer. The first set of key test parameters used was as follows: liquid capacity = 4.5–4.8 ng (i.e., approximately 4.5 ng), droplet velocity = 6–7 m / sec, frequency = 5 kHz, voltage = 16–20 V, and print temperature = 20°C–40°C. The second set of key test parameters used was as follows: liquid capacity = 8.5–9 ng (i.e., approximately 9 ng), droplet velocity = 9–11 m / sec, frequency = 5 kHz, voltage = 24–27 V, and print temperature = 20°C–40°C. The print parameter was 600 × 600 dpi printing. Measurements were performed using a PIAS II instrument, a personal image analysis system with a digital magnifying glass. To measure the dot size and diameter, a high-resolution optical module with a field of view of approximately 3.2 mm × 2.4 mm and approximately 5 μm / pixel was used. The results are shown in Tables 4 (first set) and 5 (second set). In addition, the inkjet ink composition prepared using the latex of Example 1 was continuously sprayed for >2.5 hours, during which time the faceplate remained clean and the nozzles did not clog. The ink droplets also maintained their spherical and circular shapes.
[0099] [Table 4]
[0100] [Table 5]
[0101] The results show that the aqueous inkjet ink composition made from the latex of Example 1, although not containing a water-soluble resin, exhibits printing performance equal to or better than the comparative inkjet ink composition, demonstrating excellent film-forming ability. At the same time, the water fastness of the aqueous inkjet ink composition made from the latex of Example 1 is significantly greater than that of the comparative inkjet ink composition. Specifically, it is 3 to 4 times better than the aqueous inkjet ink composition made from the latex of Comparative Example 5. Therefore, this disclosure encompasses aqueous inkjet ink compositions that exhibit a wet friction resistance of at least 10, 15, or 20 as described above when measured using a droplet of about 4.5 ng of ink, or a wet friction resistance of at least 25, 30, or 35 as described above when measured using a droplet of about 9 ng of ink.
[0102] The term “exemplary” is used herein to mean an example, case, or representation. Any embodiment or design described herein as “exemplary” is not necessarily construed as being preferable or advantageous to other embodiments or designs. Furthermore, for the purposes of this disclosure, unless otherwise specified, “a” or “an” means “one or more.”
[0103] Where not already included, all numerical values of parameters in this disclosure are referred to by the term “approximately,” meaning approximate. This includes variations inherent in the measurement of the relevant parameters as understood by those skilled in the art. This also includes the exact values of the disclosed numerical values and the rounded values of the disclosed numerical values.
[0104] The foregoing description of exemplary embodiments of the Disclosure is provided for illustrative and explanatory purposes only. It is not intended to be exhaustive or to limit the Disclosure to the exact form disclosed, and modifications and variations are possible in light of the above teachings or may be obtained from practices of the Disclosure. Embodiments are selected and described in order to illustrate the principles of the Disclosure and to enable those skilled in the art to utilize the Disclosure in various embodiments as a practical application of the Disclosure, and with various modifications suitable for the particular intended use. The scope of the Disclosure is intended to be defined by the claims and equivalents thereof appended herein.
Claims
1. 1. A method for forming a latex, comprising: adding a monomer emulsion comprising water, a monomer, an acidic monomer, a hydrophilic monomer, a difunctional monomer, a first reactive surfactant, and a chain transfer agent at a feed rate over a period of time to a reactive surfactant solution comprising water, a second reactive surfactant, and an initiator, whereby the monomers in the monomer emulsion undergo a polymerization reaction to form resin particles in a latex; the reactive surfactant solution does not include any monomer other than the second reactive surfactant, the reactive surfactant solution does not include any resin seeds, the monomer emulsion does not include any resin seeds; The method further comprising the step of: said latex being characterized by a solids content of about 30% and a viscosity in the range of about 10 cP to about 100 cP when measured at room temperature.
2. The method of claim 1 , wherein the hydrophilic monomer comprises a hydroxyl moiety, a glycol moiety, or both.
3. 2. The method of claim 1, wherein the hydrophilic monomer is selected from hydroxyethyl (meth)acrylate, n-hydroxyethyl (meth)acrylamide, hydroxypropyl (meth)acrylate, hydroxypropyl (meth)acrylamide, ethylene glycol (meth)acrylate, propylene glycol (meth)acrylate, poly(ethylene glycol) (meth)acrylate, and poly(propylene glycol) (meth)acrylate.
4. The method of claim 1, wherein the hydrophilic monomer is poly(ethylene glycol) methacrylate having a molecular weight ranging from about 185 g / mol to about 1500 g / mol.
5. The method of claim 4, wherein the molecular weight ranges from about 360 g / mol to about 1500 g / mol.
6. The method of claim 1 , wherein the difunctional monomer is poly(ethylene glycol) diacrylate.
7. 2. The method of claim 1, wherein the monomer emulsion comprises styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate, polyethylene glycol diacrylate, an anionic ether sulfate reactive surfactant, and the chain transfer agent.
8. The method of claim 1 , wherein the acidic monomer, the hydrophilic monomer, and the difunctional monomer are present in an amount ranging from about 10% to about 30% by weight.
9. The method of claim 8, wherein the difunctional monomer is present in an amount ranging from about 0.01% to about 0.8% by weight.
10. The method of claim 1, wherein the resin particles of the latex are further characterized by a glass transition temperature, Tg, in the range of about 35°C to about 100°C.
11. 2. The method of claim 1, wherein the monomer emulsion comprises one or more of the monomers, one or more of the acidic monomers, one or more of the hydrophilic monomers, one or more of the difunctional monomers, one or more first reactive surfactants, and one or more of the chain transfer agents.
12. 2. The method of claim 1, wherein said monomer emulsion consists of styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate, polyethylene glycol diacrylate, an anionic ether sulfate reactive surfactant, and said chain transfer agent.
13. The method of claim 1 , wherein the reactive surfactant solution further comprises silica nanoparticles.
14. A latex comprising water and resin particles comprising the polymerization product of reactants including a monomer, an acidic monomer, a monofunctional hydrophilic monomer, a difunctional monomer, and a reactive surfactant, said latex being characterized by a viscosity in the range of about 10 cP to about 100 cP when measured at about 30% solids content and room temperature.
15. The latex of claim 14, wherein the viscosity is in the range of about 15 cP to about 40 cP.
16. 15. The latex of claim 14, wherein the monofunctional hydrophilic monomer is selected from hydroxyethyl (meth)acrylate, n-hydroxyethyl (meth)acrylamide, hydroxypropyl (meth)acrylate, hydroxypropyl (meth)acrylamide, ethylene glycol (meth)acrylate, propylene glycol (meth)acrylate, poly(ethylene glycol) (meth)acrylate, poly(propylene glycol) (meth)acrylate, and combinations thereof.
17. 15. The latex of claim 14, wherein the monofunctional hydrophilic monomer is a poly(ethylene glycol) methacrylate having a molecular weight ranging from about 185 g / mol to about 1500 g / mol.
18. The latex of claim 17, wherein the molecular weight is in the range of about 360 g / mol to about 1500 g / mol.
19. The latex of claim 14, wherein the reactants include styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate, poly(ethylene glycol) diacrylate, and an anionic ether sulfate reactive surfactant.
20. 15. The latex of claim 14, wherein the acidic monomer, the monofunctional hydrophilic monomer, and the difunctional monomer are present in an amount ranging from about 10% to about 30% by weight.
21. The latex of claim 20, wherein the acidic monomer, the monofunctional hydrophilic monomer, and the difunctional monomer are present in an amount ranging from about 15% to about 30% by weight.
22. 21. The latex of claim 20, wherein the difunctional monomer is present in an amount ranging from about 0.01% to about 0.8% by weight.
23. 15. The latex of claim 14, wherein the resin particles of the latex are further characterized by a glass transition temperature, Tg, in the range of from about 35°C to about 100°C.
24. The latex of claim 23, wherein the glass transition temperature Tg is in the range of about 50°C to about 80°C.
25. The latex of claim 14, wherein the reactants comprise one or more monomers, one or more acidic monomers, one or more monofunctional hydrophilic monomers, one or more difunctional monomers, one or more reactive surfactants, and one or more initiators.
26. The latex of claim 14, wherein the reactants consist of styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate, poly(ethylene glycol) diacrylate, an anionic ether sulfate reactive surfactant, and one or more initiators.
27. 15. The latex of claim 14, wherein the latex further comprises silica nanoparticles.
28. A latex comprising water and resin particles comprising the polymerization product of reactants including a monomer, an acidic monomer, a monofunctional hydrophilic monomer, a difunctional monomer, and a reactive surfactant, wherein the acidic monomer, the monofunctional hydrophilic monomer, and the difunctional monomer are present in an amount ranging from about 15% to about 30% by weight, and the latex is characterized by a solids content of about 30% and a viscosity ranging from about 15 cP to about 40 cP when measured at room temperature.
29. The latex of claim 28, wherein the reactants include styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate, poly(ethylene glycol) diacrylate, and an anionic ether sulfate reactive surfactant.
30. The latex of claim 29, wherein the poly(ethylene glycol) methacrylate has a molecular weight in the range of about 360 g / mol to about 1500 g / mol.
31. The latex of claim 30, further comprising silica nanoparticles.
32. A latex comprising water, silica nanoparticles, and resin particles comprising the polymerization product of reactants consisting of one or more monomers, one or more acidic monomers, one or more monofunctional hydrophilic monomers, one or more difunctional monomers, one or more reactive surfactants, and one or more initiators, said latex being characterized by a viscosity in the range of about 15 cP to about 40 cP when measured at about 30% solids content and room temperature.
33. The latex of claim 32, wherein the reactants consist of styrene, an alkyl acrylate, methacrylic acid, styrene sulfonic acid, poly(ethylene glycol) methacrylate having a molecular weight in the range of about 360 g / mol to about 1500 g / mol, poly(ethylene glycol) diacrylate, an anionic ether sulfate reactive surfactant, and one or more initiators.