Light-absorbing anisotropic film, optical film and optical laminate
A light-absorbing anisotropic film with specific dichroic dyes and polymerizable liquid crystal compounds addresses the issue of image clarity degradation in organic EL displays under temperature stress, ensuring sharpness and clarity through optimized absorbance ratios and thickness.
Patent Information
- Application Number
- JP2024025649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-09
AI Technical Summary
Existing light-absorbing anisotropic films used in organic EL display devices suffer from decreased image clarity when exposed to harsh temperature environments, as they fail to maintain sharpness and clarity due to the properties of vertically aligned liquid crystal cured films.
A light-absorbing anisotropic film composed of a composition containing one or more dichroic dyes and a polymerizable liquid crystal compound, with specific liquid crystal compounds exhibiting smectic liquid crystal phases and multiple polymerizable groups, formulated to meet certain absorbance ratios and thickness criteria, enhancing stability and clarity under temperature variations.
The film effectively suppresses deterioration in image clarity even under harsh temperature conditions, maintaining sharpness and reducing haze, thus improving display quality.
Smart Images

Figure 2024139702000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optically absorptive anisotropic film, and further to an optical film and an optical laminate including the same. [Background technology]
[0002] In an organic EL (electroluminescence) display device, in order to reduce the hue difference between the front hue when viewed from the front and the oblique hue when viewed from an oblique angle during white display, it is known to use a laminate having a vertically aligned liquid crystal cured film containing a dichroic dye and a horizontally aligned retardation film (for example, Patent Document 1). Patent Document 1 describes that the vertically aligned liquid crystal cured film is formed using a dichroic dye and a polymerizable liquid crystal compound exhibiting two types of smectic liquid crystal phases. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-076920 A Summary of the Invention [Problem to be solved by the invention]
[0004] When a vertically aligned liquid crystal cured film formed using two types of polymerizable liquid crystal compounds exhibiting a smectic liquid crystal phase is applied to a display device such as an organic electroluminescence display device, the clarity of the image display may decrease when the display device is exposed to a harsh temperature environment.
[0005] An object of the present invention is to provide an optically absorptive anisotropic film capable of suppressing a decrease in the clarity of an image display even when exposed to a severe temperature environment, and an optical film and an optical laminate including the same. [Means for solving the problem]
[0006] The present invention provides the following optically absorptive anisotropic film, optical film, and optical laminate. [1] A light absorption anisotropic film formed from a composition containing one or more dichroic dyes and a polymerizable liquid crystal compound, the polymerizable liquid crystal compound includes a first liquid crystal compound and a second liquid crystal compound different from the first liquid crystal compound, each of the first liquid crystal compound and the second liquid crystal compound exhibits a smectic liquid crystal phase and contains two or more polymerizable groups in the molecule; The optically absorptive anisotropic film satisfies the relationships of the following formulas (1) and (2): 0.001≦Ax≦0.3 (1) Ax(z=50°) / Ax≧5 (2) [In formulas (1) and (2), Ax is the absorbance of the optically absorptive anisotropic film at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less, and represents the absorbance of linearly polarized light oscillating in the x-axis direction. Ax (z=50°) is the absorbance at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less when the optically absorptive anisotropic film is rotated 50° around the y axis as the rotation axis, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Here, the x-axis is an arbitrary direction within the plane of the optically absorptive anisotropic film, The y-axis is a direction perpendicular to the x-axis within the plane of the optically absorptive anisotropic film. [2] The optically absorptive anisotropic film according to [1], wherein a total content of the first liquid crystal compound and the second liquid crystal compound is 99 mass % or more based on a total amount of the polymerizable liquid crystal compound. [3] The optically absorptive anisotropic film according to [1] or [2], wherein the polymerizable groups are each a (meth)acryloyl group. [4] The optically absorptive anisotropic film according to any one of [1] to [3], wherein the composition further contains a non-liquid crystal compound having a reactive group. [5] The optically absorptive anisotropic film according to any one of [1] to [4], having a thickness of 0.1 μm or more and 3.0 μm or less. [6] The optically absorptive anisotropic film according to any one of [1] to [5], having a haze of 2.5% or less. [7] The first liquid crystal compound is a compound (a) represented by the following formula (a): The optically absorptive anisotropic film according to any one of [1] to [6], wherein the second liquid crystal compound is a compound (b) represented by the following formula (b): P1-F1-B1-G1-D1-G2-D2-G3-B2-F2-P2 (a) P3-F3-B3-G4-D3-G5-D4-G6-B4-F4-P4 (b) [In the formula (a) and the formula (b), D1 to D4 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -C(=S)-O-, -OC(=S)-, -OC(=S)-O-, or -CO-NR 11 -, -NR 12 -CO- or a single bond, R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, B1 to B4 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, or -CO-NR 11 -, -NR 12 -CO- or a single bond, R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, G1 to G6 each independently represent a divalent alicyclic hydrocarbon group having 3 to 16 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and a hydrogen atom contained in the alicyclic hydrocarbon group or the aromatic hydrocarbon group is not optionally substituted with a halogen atom, -R 13 , -OR 13 , cyano, or nitro; R 13 represents an alkyl group having 1 to 4 carbon atoms, and a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, F1 to F4 each independently represent an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group is -OR 14 or halogen atom, R 14represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, and -CH- contained in the alkanediyl group may be substituted with -O- or -CO-, P1 to P4 each represent a polymerizable group.] [8] The optically absorptive anisotropic film according to [7], wherein in the formulae (a) and (b), G1 and G4 are the same group, D1 and D3 are the same group, G2 and G5 are the same group, D2 and D4 are the same group, and G3 and G6 are the same group. [9] In the formulas (a) and (b), when the total number of carbon atoms contained in F1 and the total number of carbon atoms contained in F2 is C(a) and the total number of carbon atoms contained in F3 and the total number of carbon atoms contained in F4 is C(b), The optically absorptive anisotropic film according to [7] or [8], wherein C(a) is greater than C(b).
[10] An optical film comprising the optically absorptive anisotropic film according to any one of [1] to [9] and a substrate layer.
[11] An optical laminate comprising the optically absorptive anisotropic film according to any one of [1] to [9] or the optical film according to
[10] , and an elliptically polarizing plate. Effect of the Invention
[0007] According to the present invention, it is possible to provide an optically absorptive anisotropic film that can suppress a decrease in the clarity of an image display even when exposed to a severe temperature environment, as well as an optical film and an optical laminate including the same. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view illustrating an optical film according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view that illustrates an optical laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, preferred embodiments of the optically absorptive anisotropic film, the optical film, and the optical laminate will be described. In this specification, a numerical range such as "x to y" refers to an upper limit and a lower limit, and represents a numerical range of "x or more and y or less", unless otherwise specified.
[0010] <Light-absorbing anisotropic film> The optically absorptive anisotropic film is formed from a composition (hereinafter sometimes referred to as "optically absorptive anisotropic film-forming composition") containing one or more dichroic dyes and a polymerizable liquid crystal compound, and satisfies the relationships of the following formulas (1) and (2). The polymerizable liquid crystal compound contains a first liquid crystal compound and a second liquid crystal compound different from the first liquid crystal compound. Both the first liquid crystal compound and the second liquid crystal compound exhibit a smectic liquid crystal phase and contain two or more polymerizable groups in the molecule. 0.001≦Ax≦0.3 (1) Ax(z=50°) / Ax≧5 (2) [In formulas (1) and (2), Ax is the absorbance of the optically absorptive anisotropic film at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Ax (z=50°) is the absorbance at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less when the optically absorptive anisotropic film is rotated 50° around the y axis as the rotation axis, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Here, the x-axis is an arbitrary direction in the plane of the optically absorptive anisotropic film, The y-axis is a direction perpendicular to the x-axis in the plane of the optically absorptive anisotropic film.
[0011] The optically absorptive anisotropic film is formed from a composition for forming an optically absorptive anisotropic film, which contains a dichroic dye and a polymerizable liquid crystal compound. The optically absorptive anisotropic film can be formed by polymerizing the polymerizable liquid crystal compound in the composition for forming an optically absorptive anisotropic film. The optically absorptive anisotropic film can contain a polymer of a polymerizable liquid crystal compound, and can contain the polymer and a dichroic dye. When a compound that can be polymerized with a polymerizable liquid crystal compound other than the polymerizable liquid crystal compound (hereinafter, sometimes referred to as a "polymerizable compound") is present in the composition for forming an optically absorptive anisotropic film, the polymer of the polymerizable liquid crystal compound may be a copolymer of the polymerizable liquid crystal compound and the polymerizable compound. Examples of the polymerizable compound include a dichroic dye having a polymerizable group, and a non-liquid crystal compound described later.
[0012] The composition for forming an optically absorptive anisotropic film contains, as polymerizable liquid crystal compounds, a first liquid crystal compound and a second liquid crystal compound different from the first liquid crystal compound. Therefore, the optically absorptive anisotropic film can contain, as a polymer of the polymerizable liquid crystal compound, a copolymer of the first liquid crystal compound and the second liquid crystal compound, or may contain a copolymer of the first liquid crystal compound, the second liquid crystal compound, and a polymerizable compound.
[0013] As described above, both the first liquid crystal compound and the second liquid crystal compound exhibit a smectic liquid crystal phase and contain two or more polymerizable groups in the molecule. The optically absorptive anisotropic film formed from the optically absorptive anisotropic film-forming composition containing two kinds of such polymerizable liquid crystal compounds (i.e., containing the first liquid crystal compound and the second liquid crystal compound) exhibits a smectic liquid crystal phase, and compared to an optically absorptive anisotropic film formed from a composition containing a polymerizable liquid crystal compound having one polymerizable group in the molecule (hereinafter, sometimes referred to as a "monofunctional polymerizable liquid crystal compound"), it can suppress an increase in haze even when exposed to a severe temperature environment. Therefore, when the optically absorptive anisotropic film of this embodiment is applied to a display device and exposed to a severe temperature environment, it can suppress a decrease in the clarity of the image display.
[0014] The reason for this is presumed to be as follows. The first liquid crystal compound and the second liquid crystal compound contain two or more polymerizable groups in the molecule, and therefore are more reactive than monofunctional polymerizable liquid crystal compounds. Therefore, the optically absorptive anisotropic film of the present embodiment is considered to have a smaller amount of unreacted polymerizable liquid crystal compound remaining than an optically absorptive anisotropic film formed from a composition containing a monofunctional polymerizable liquid crystal compound. As a result, it is presumed that the optically absorptive anisotropic film of the present embodiment can suppress adverse effects caused by unreacted polymerizable liquid crystal compounds remaining in the film when exposed to a severe temperature environment.
[0015] The content of the polymerizable liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film is preferably 40% by mass or more and 99.9% by mass or less, and may be 60% by mass or more and 99% by mass or less, or may be 70% by mass or more and 99% by mass or less, based on the total amount of the solid content of the composition for forming an optically absorptive anisotropic film. When the content of the polymerizable liquid crystal compound in the composition for forming an optically absorptive anisotropic film is within the above range, the orientation of the polymerizable liquid crystal compound when forming an optically absorptive anisotropic film tends to be high. In this specification, the solid content of the composition means all components of the composition excluding volatile components such as organic solvents.
[0016] The total content of the first liquid crystal compound and the second liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film is preferably 99% by mass or more, more preferably 100% by mass, based on the total amount of the polymerizable liquid crystal compound. When the total content of the first liquid crystal compound and the second liquid crystal compound in the composition for forming an optically absorptive anisotropic film is within the above range, it becomes easier to further suppress an increase in haze of the optically absorptive anisotropic film when exposed to a severe temperature environment. Details of the composition for forming an optically absorptive anisotropic film, the dichroic dye, the first liquid crystal compound, and the second liquid crystal compound will be described later.
[0017] The absorbance Ax of the optically absorptive anisotropic film means the absorbance in the front direction in the plane of the optically absorptive anisotropic film. The smaller the value of the absorbance Ax, the less coloring of the optically absorptive anisotropic film in the front direction. When the absorbance Ax exceeds 0.3, the coloring of the optically absorptive anisotropic film in the front direction becomes strong, so that the front hue tends to be inferior when applied to an organic EL display device in combination with an elliptically polarizing plate described later. Therefore, the absorbance Ax in formula (1) is preferably 0.001 or more and 0.2 or less, more preferably 0.001 or more and 0.1 or less, and even more preferably 0.001 or more and 0.05 or less.
[0018] In formula (2), the larger the value of Ax(z=50°) / Ax, the more excellent the light absorption anisotropy is. For example, the value may be greater than 5, 7 or more, 10 or more, or 50 or less.
[0019] Since the optically absorptive anisotropic film that satisfies the relationship of the above formula (2) is considered to have the absorption axis of the dichroic dye oriented perpendicular to the plane of the film, the optically absorptive anisotropic film can effectively absorb light from an oblique direction. The optically absorptive anisotropic film that satisfies the relationship of the above formula (2) can be adjusted, for example, by the thickness of the optically absorptive anisotropic film, the conditions of the manufacturing process of the optically absorptive anisotropic film (described later), and the types or contents of the dichroic dye and polymerizable liquid crystal compound contained in the optically absorptive anisotropic film-forming composition that forms the optically absorptive anisotropic film.
[0020] The above Ax(z=50°) means the oblique absorbance of the light absorbing anisotropic film, and can be appropriately selected according to the light leaking obliquely from the display device. Ax(z=50°) is preferably 1.0 or less, more preferably 0.5 or less, and even more preferably 0.3 or less. Ax(z=50°) is usually 0.001 or more, may be 0.003 or more, and is 0.01 or more if necessary.
[0021] The thickness of the optically absorptive anisotropic film is preferably 0.1 μm or more and 3.0 μm or less, more preferably 0.3 μm or more and 2.5 μm or less, and even more preferably 0.5 μm or more and 2.0 μm or less. By having the thickness of the optically absorptive anisotropic film within the above range, it is easy to suppress the increase in haze and the decrease in the clarity of the image display even when exposed to a severe temperature environment. In addition, the smaller the thickness of the optically absorptive anisotropic film, the easier it is to suppress the increase in haze and the decrease in the clarity of the image display when exposed to a severe temperature environment.
[0022] The haze of the optically absorptive anisotropic film is preferably 2.5% or less, more preferably 2.3% or less, further preferably 2.0% or less, and is usually 0.1% or more.
[0023] When the haze of the optically absorptive anisotropic film is the initial haze H0, and the haze of the optically absorptive anisotropic film after the durability test described in the examples below is the haze after the durability test H1, the haze difference ΔH (=H1-H0) between the initial haze H0 and the haze H1 after the durability test is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. By having the haze difference ΔH within the above range, the optically absorptive anisotropic film is easy to suppress the decrease in the clarity of the image display when exposed to a severe temperature environment.
[0024] (Light-absorbing anisotropic film-forming composition (composition)) The composition for forming an optically absorptive anisotropic film contains a dichroic dye and a polymerizable liquid crystal compound as described above. The composition for forming an optically absorptive anisotropic film may further contain a non-liquid crystal compound having a reactive group in addition to the dichroic dye and the polymerizable liquid crystal compound. The details of the non-liquid crystal compound having a reactive group will be described later.
[0025] The composition for forming an optically absorptive anisotropic film may contain a solvent in order to form an optically absorptive anisotropic film by coating. Generally, polymerizable liquid crystal compounds have high viscosity, so by dissolving them in a solvent to form an optically absorptive anisotropic film-forming composition containing a solvent, it becomes easy to apply the composition to the first base layer described below, and as a result, it is often easy to form an optically absorptive anisotropic film. Details of the solvent will be described later.
[0026] The composition for forming an optically absorbing anisotropic film may contain additives such as a polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator, a leveling agent, an antioxidant, and a photosensitizer, in addition to the above-mentioned components. The composition for forming an optically absorbing anisotropic film may further contain an alignment promoter. Details of these additives will be described later.
[0027] The composition for forming an optically absorptive anisotropic film can be obtained by stirring a dichroic dye and a polymerizable liquid crystal compound, and, if necessary, additives such as a non-liquid crystal compound having a reactive group, a solvent, an alignment promoter, a polymerization initiator, and a leveling agent.
[0028] (Polymerizable liquid crystal compound) The polymerizable liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film is used to align a dichroic dye by host-guest interaction. The polymerizable liquid crystal compound has one or more polymerizable groups in the molecule and has liquid crystal properties.
[0029] The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and a (meth)acryloyl group and a (meth)acryloyloxy group are more preferred. The liquid crystal property may be a thermotropic liquid crystal or a lyotropic liquid crystal, but when mixed with the above-mentioned dichroic dye, a thermotropic liquid crystal is preferred. In this specification, a (meth)acryloyl group means at least one of an acryloyl group and a methacryloyl group. The same applies to the notation of (meth)acrylic, etc.
[0030] When forming a polymer of a polymerizable liquid crystal compound by polymerization reaction and expressing light absorption anisotropy characteristics as a film containing the polymer and a dichroic dye, the liquid crystal state shown by the polymerizable liquid crystal compound is a smectic phase, and it is preferable that the polymerizable liquid crystal compound is a high-order smectic phase from the viewpoint of high optical performance. Among them, a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferable, and a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic F phase, or a smectic I phase is even more preferable. When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these high-order smectic phases, a light absorption anisotropic film with higher light absorption anisotropy characteristics can be produced. In this way, the optically absorptive anisotropic film having high optical absorption anisotropy characteristics is one in which a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase is obtained in X-ray diffraction measurement. The Bragg peak is a peak derived from a periodic structure of molecular orientation, and the optically absorptive anisotropic film can have a periodic interval of 3 to 6 Å. It is preferable that the optically absorptive anisotropic film contains a polymer of a polymerizable liquid crystal compound oriented in a smectic phase state, from the viewpoint of obtaining higher optical absorption anisotropy characteristics.
[0031] The polymerizable liquid crystal compound may be a monomer, an oligomer in which a polymerizable group is polymerized, or a polymer. As such a polymerizable liquid crystal compound, a known compound can be used, for example, those described in JP-A-2020-76920 and JP-A-6728581.
[0032] (First liquid crystal compound and second liquid crystal compound) The first liquid crystal compound and the second liquid crystal compound are polymerizable liquid crystal compounds that exhibit a smectic liquid crystal phase and contain two or more polymerizable groups in the molecule. The first liquid crystal compound and the second liquid crystal compound may differ in part of their chemical structures, and may differ in the polymerizable groups or in chemical structures other than the polymerizable groups.
[0033] The number of polymerizable groups possessed by the first liquid crystal compound and the second liquid crystal compound may be independently 2, 3, or 4 or more, but is preferably 2. The two or more polymerizable groups possessed by the first liquid crystal compound and the second liquid crystal compound are preferably both (meth)acryloyl groups.
[0034] The first liquid crystal compound is preferably a compound (a) represented by the following formula (a): The second liquid crystal compound is preferably a compound (b) represented by the following formula (b): P1-F1-B1-G1-D1-G2-D2-G3-B2-F2-P2 (a) P3-F3-B3-G4-D3-G5-D4-G6-B4-F4-P4 (b) [In the formula (a) and the formula (b), D1 to D4 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -C(=S)-O-, -OC(=S)-, -OC(=S)-O-, or -CO-NR 11 -, -NR 12 -CO- or a single bond, R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, B1 to B4 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, or -CO-NR 11 -, -NR 12 -CO- or a single bond, R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, G1 to G6 each independently represent a divalent alicyclic hydrocarbon group having 3 to 16 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and a hydrogen atom contained in the alicyclic hydrocarbon group or the aromatic hydrocarbon group is not optionally substituted with a halogen atom, -R 13 , -OR 13 , cyano, or nitro; R 13 represents an alkyl group having 1 to 4 carbon atoms, and a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, F1 to F4 each independently represent an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group is -OR 14 or halogen atom, R 14 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, and -CH- contained in the alkanediyl group may be substituted with -O- or -CO-, P1 to P4 each represent a polymerizable group.]
[0035] D1 and D3 are each independently preferably -O-, -S-, -CO-O-, -O-CO-, or -O-CO-O-, and more preferably -CO-O-. D2 and D4 are each independently preferably -O-, -S-, -CO-O-, -O-CO-, or -O-CO-O-, and more preferably -O-CO-.
[0036] B1 and B3 each independently preferably represent -O-, -S-, -CO-O-, or -O-CO-, and more preferably represent -O- or -O-CO-. B2 and B4 each independently preferably represent -O-, -S-, -CO-O-, or -O-CO-, and more preferably represent -O- or -CO-O-.
[0037] The number of carbon atoms in the divalent alicyclic hydrocarbon groups G1 to G6 is preferably 5 to 12, and more preferably 5 or 6. The divalent alicyclic hydrocarbon group G1 to G6 is preferably a cyclohexane-1,4-diyl group. The number of carbon atoms in the divalent aromatic hydrocarbon groups G1 to G6 is preferably 6 to 10, and more preferably 6. The divalent aromatic hydrocarbon groups G1 to G6 are preferably 1,4-phenylene groups.
[0038] F1 to F4 are each independently preferably a linear alkanediyl group having 1 to 12 carbon atoms, and -CH2- contained in the alkanediyl group may be replaced by -O- or -CO-. F1 to F4 each independently include linear alkanediyl groups having 1 to 12 carbon atoms, such as a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a nonane-1,9-diyl group, a decane-1,10-diyl group, an undecane-1,11-diyl group, and a dodecane-1,12-diyl group; -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2-, and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-.
[0039] The polymerizable groups P1 to P4 include those described as the polymerizable groups of the polymerizable liquid crystal compound. The polymerizable groups P1 to P4 may all be the same, all may be different, or some may be the same and some may be different. It is preferable that all of the polymerizable groups P1 to P4 are (meth)acryloyl groups.
[0040] When the first liquid crystal compound is compound (a) and the second liquid crystal compound is compound (b), it is preferable that in the above formulae (a) and (b), G1 and G4 are the same group, D1 and D3 are the same group, G2 and G5 are the same group, D2 and D4 are the same group, and G3 and G6 are the same group (hereinafter, this may be referred to as "condition [i]"). In addition to condition [i], it is more preferable that P1 to P4 in the above formulae (a) and (b) are the same group, and it is particularly preferable that P1 to P4 are (meth)acryloyl groups. In this case, in the first liquid crystal compound and the second liquid crystal compound, in the above formulae (a) and (b), it is preferable that F1 and F3 are different groups, B1 and B3 are different groups, B2 and B4 are different groups, and / or F2 and F4 are different groups, and among these, it is more preferable that F1 and F3 are different groups and / or F2 and F4 are different groups.
[0041] When the first liquid crystal compound is a compound (a) and the second liquid crystal compound is a compound (b), in the above formulas (a) and (b), the total number of carbon atoms contained in F1 and F2 is C(a), and the total number of carbon atoms contained in F3 and F4 is C(b). It is preferable that C(a) is larger than C(b) (hereinafter, this may be referred to as "condition [ii]"). When -CH2- constituting the alkanediyl group representing F1 to F4 is replaced with -O- or -CO-, the number of carbon atoms of F1 to F4 is the number of carbon atoms of the alkanediyl group before being replaced with these functional groups. It is more preferable that the first liquid crystal compound and the second liquid crystal compound simultaneously satisfy conditions [i] and [ii], it is even more preferable that conditions [i] and [ii] are simultaneously satisfied and P1 to P4 are the same group, and it is particularly preferable that conditions [i] and [ii] are simultaneously satisfied and P1 to P4 are (meth)acryloyl groups.
[0042] Examples of the compounds (a) and (b) include compounds represented by the following formulae: In the following formulae, k1 and k2 each independently represent an integer of 1 to 12. [ka] [ka] [ka]
[0043] (dichroic dye) The dichroic dye is a dye having different absorbance in the long axis direction of the molecule and absorbance in the short axis direction of the molecule. The dichroic dye preferably has a property of absorbing visible light, and more preferably has a maximum absorption wavelength (λmax) in the wavelength range of 380 to 680 nm.
[0044] Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, among which bisazo dyes and trisazo dyes are preferred. The dichroic dyes may be used alone or in combination of two or more kinds, but it is preferred to use two or more kinds in combination according to the wavelength range in which the light absorption anisotropy is required in the light absorption anisotropic film.
[0045] An example of the azo dye is a compound represented by the formula (c). T 1 -A 1 (-N=NA 2 ) p -N=NA 3 -T 2 (c) [In formula (c), A 1 , A 2 , and A 3represent each independently an optionally substituted 1,4-phenylene group, an optionally substituted naphthalene-1,4-diyl group, an optionally substituted benzoic acid phenyl ester group, an optionally substituted 4,4'-stilbenylene group, or an optionally substituted divalent heterocyclic group, T 1 and T 2 represents an electron withdrawing group or an electron releasing group, and is located at an angle of substantially 180° to the plane of the azo bond. p represents an integer of 0 to 4, and when p is 2 or more, each A 2 may be the same or different from each other. As long as the compound exhibits absorption in the visible light region, the -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond.
[0046] The content of the dichroic dye contained in the composition for forming an optically absorptive anisotropic film is preferably 0.1% by mass or more and 30% by mass or less, or may be 0.5% by mass or more and 20% by mass or less, or may be 1% by mass or more and 10% by mass or less, or may be 1% by mass or more and 5% by mass or less, based on the total amount of the solid content of the composition for forming an optically absorptive anisotropic film. When the composition for forming an optically absorptive anisotropic film contains two or more kinds of dichroic dyes, the content of the dichroic dyes refers to the total amount.
[0047] The content of the dichroic dye contained in the composition for forming an optically absorptive anisotropic film (the total amount when multiple types are contained) is usually 1 part by mass to 60 parts by mass, preferably 1 part by mass to 40 parts by mass, and more preferably 1 part by mass to 20 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound, from the viewpoint of obtaining good optical absorption properties. If the content of the dichroic dye is less than this range, the optical absorption becomes insufficient and sufficient optical absorption anisotropy properties cannot be obtained, whereas if the content is more than this range, the alignment of the liquid crystal molecules of the polymerizable liquid crystal compound may be hindered.
[0048] (Non-liquid crystal compound having a reactive group) A non-liquid crystal compound having a reactive group (hereinafter, sometimes referred to as a "non-liquid crystal compound") is a compound having a reactive group and not having liquid crystallinity. Examples of reactive groups that non-liquid crystal compounds have include vinyl groups, vinyloxy groups, 1-chlorovinyl groups, isopropenyl groups, 4-vinylphenyl groups, (meth)acryloyl groups, (meth)acryloyloxy groups, oxiranyl groups, and oxetanyl groups. Among these, preferred reactive groups are (meth)acryloyl groups, (meth)acryloyloxy groups, vinyloxy groups, oxiranyl groups, and oxetanyl groups, more preferred reactive groups are (meth)acryloyl groups and (meth)acryloyloxy groups, and even more preferred polymerizable groups are (meth)acryloyloxy groups. The reactive groups in non-liquid crystal compounds may be one type or a combination of two or more types, but are preferably the same as the polymerizable groups in polymerizable liquid crystal compounds.
[0049] The number of reactive groups possessed by the non-liquid crystal compound is not particularly limited and may be, for example, 1 to 20, but from the viewpoint of easier enhancement of the film strength of the optically absorptive anisotropic film, the number is preferably 2 to 10, more preferably 3 to 6. When the non-liquid crystal compound has two or more polymerizable groups, the polymerizable groups may be the same or different from each other.
[0050] Examples of the non-liquid crystal compound include monofunctional (meth)acrylates and polyfunctional (meth)acrylates. Since the monofunctional acrylates and polyfunctional acrylates as non-liquid crystal compounds are non-liquid crystal, they preferably do not have a mesogen structure. The monofunctional acrylates and polyfunctional acrylates may contain a urethane structure, an amino structure, an epoxy structure, an ethylene glycol structure, and / or a polyester structure in the molecule.
[0051] (solvent) The solvent that may be contained in the composition for forming an optically absorptive anisotropic film is preferably one that can completely dissolve the polymerizable liquid crystal compound, and is preferably a solvent that is inactive to the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more.
[0052] The content of the solvent in the composition for forming an optically absorptive anisotropic film is preferably 50 to 98% by mass relative to the total amount of the composition for forming an optically absorptive anisotropic film. In other words, the content of the solid content in the composition for forming an optically absorptive anisotropic film is preferably 2 to 50% by mass, more preferably 5 to 30% by mass. When the content of the solid content is 50% by mass or less, the viscosity of the composition for forming an optically absorptive anisotropic film is low, so that the optically absorptive anisotropic film is easily formed to a substantially uniform thickness, and the optically absorptive anisotropic film tends to be less prone to unevenness. The content of the solid content can be determined in consideration of the thickness of the optically absorptive anisotropic film to be produced.
[0053] (Additives) The composition for forming an optically absorptive anisotropic film may contain a polymerization initiator. The polymerization initiator is used when the composition for forming an optically absorptive anisotropic film contains a compound involved in a polymerization reaction such as a polymerizable liquid crystal compound, and is a compound capable of initiating the polymerization reaction of the compound. As the polymerization initiator for initiating the polymerization reaction of the polymerizable liquid crystal compound, a photopolymerization initiator that generates active radicals by the action of light is preferred from the viewpoint of not depending on the phase state of the thermotropic liquid crystal.
[0054] The photopolymerization initiator may be any known photopolymerization initiator as long as it is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound or the like. Specifically, photopolymerization initiators capable of generating active radicals or acids under the action of light are included, and among these, photopolymerization initiators that generate radicals under the action of light are preferred. The photopolymerization initiators may be used alone or in combination of two or more.
[0055] As the photopolymerization initiator, a known photopolymerization initiator can be used. For example, the photopolymerization initiator that generates active radicals is Self-cleavable benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, azo compounds, and the like; Hydrogen abstraction type benzophenone compounds, alkylphenone compounds, benzoin ether compounds, benzil ketal compounds, dibenzosuberone compounds, anthraquinone compounds, xanthone compounds, thioxanthone compounds, halogenoacetophenone compounds, dialkoxyacetophenone compounds, halogenobisimidazole compounds, halogenotriazine compounds, triazine compounds, etc. can be used.
[0056] As the photopolymerization initiator that generates an acid, an iodonium salt, a sulfonium salt, or the like can be used.
[0057] From the viewpoint of excellent reaction efficiency at low temperatures, the photopolymerization initiator is preferably a self-cleavage type photopolymerization initiator, and in particular, an acetophenone-based compound, a hydroxyacetophenone-based compound, an α-aminoacetophenone-based compound, or an oxime ester-based compound is preferred.
[0058] The content of the polymerization initiator in the composition for forming an optically absorptive anisotropic film can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, but is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the alignment of the polymerizable liquid crystal compound.
[0059] The leveling agent is an additive that adjusts the fluidity of the composition and makes the film obtained by applying the composition flatter. The light absorption anisotropic film forming composition can contain a silicon-based leveling agent, a polyacrylate-based leveling agent, or a fluorine-based leveling agent such as a perfluoroalkyl-based leveling agent.
[0060] (Method of forming optically absorptive anisotropic film) The optically absorbing anisotropic film can be formed, for example, by applying the optically absorbing anisotropic film-forming composition onto a first substrate layer (described later). The coating layer formed by applying the optically absorbing anisotropic film-forming composition is subjected to a drying treatment to remove the solvent and the like. The coating layer after the drying treatment is irradiated with active energy rays or the like to polymerize the polymerizable liquid crystal compound, thereby forming an optically absorbing anisotropic film as a cured layer (liquid crystal cured film) of the optically absorbing anisotropic film-forming composition on the first substrate layer. The optically absorbing anisotropic film-forming composition may be applied to the surface of the first substrate layer, or may be applied to the surface of a first alignment layer (described later) formed on the surface of the first substrate layer.
[0061] Examples of a method for applying the composition for forming an optically absorptive anisotropic film include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0062] It is preferable to perform a drying process on the coating layer of the composition for forming an optically absorptive anisotropic film formed on the first base layer. When the composition for forming an optically absorptive anisotropic film contains a solvent, the solvent in the coating layer can be removed by drying the coating layer. The drying method may be a known method, and may include one or more methods selected from natural drying, heat drying, ventilation drying, and reduced pressure drying.
[0063] The drying conditions in the drying process can be appropriately determined depending on the components contained in the composition for forming an optically absorptive anisotropic film. For example, the drying temperature in the drying process may be 50° C. or more and 150° C. or less, or 60° C. or more and 120° C. or less. The drying time in the drying process may be 15 seconds or more and 10 minutes or less, or 0.5 minutes or more and 5 minutes or less.
[0064] When a heat treatment is performed in the drying process, the polymerizable liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film can be oriented while removing the solvent in the coating layer by heating to a temperature equal to or higher than the liquid crystal phase transition temperature at which the polymerizable liquid crystal compound undergoes a phase transition. In particular, when a polymerizable liquid crystal compound that forms a smectic phase is oriented in a direction perpendicular to the surface of the optically absorptive anisotropic film, it is preferable to heat the composition in a temperature range where the compound transitions to a smectic phase. This allows the polymerizable liquid crystal compound to be oriented in a direction perpendicular to the surface of the optically absorptive anisotropic film, and the dichroic dye can also be oriented along with the orientation of the polymerizable liquid crystal compound.
[0065] After drying the coating layer formed on the first substrate layer, the polymerizable liquid crystal compound and the dichroic dye are oriented, and then the polymerizable liquid crystal compound is polymerized and cured by irradiating the coating layer with active energy rays, thereby forming a light absorbing anisotropic film in which the polymerizable liquid crystal compound and the dichroic dye are oriented.
[0066] Photopolymerization is preferred as a method for polymerizing the polymerizable liquid crystal compound. Photopolymerization is performed by irradiating active energy rays to a laminated structure including a coating layer in which a light absorption anisotropic film-forming composition containing a polymerizable liquid crystal compound is applied on a first base layer. The active energy rays to be irradiated are appropriately selected according to the type of polymerizable liquid crystal compound contained in the coating layer (particularly, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator when a photopolymerization initiator is contained, and the amount thereof. Specifically, one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be mentioned. Among them, ultraviolet light is preferred in terms of ease of controlling the progress of the polymerization reaction and the ability to use photopolymerization devices that are widely used in this field, and it is preferable to select the type of polymerizable liquid crystal compound so that it can be photopolymerized by ultraviolet light.
[0067] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.
[0068] The UV irradiation intensity is usually 10mW / cm 2 ~3,000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a radical polymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 mJ / cm 2 ~3,000mJ / cm 2 , preferably 50 mJ / cm 2 ~2,000mJ / cm 2 , more preferably 100 mJ / cm 2 ~1,000mJ / cm2 If the accumulated light amount is less than this range, the polymerizable liquid crystal compound is not sufficiently cured, and good transferability may not be obtained when transferring the optically absorptive anisotropic film on the first base layer to an adherend. Conversely, if the accumulated light amount is more than this range, the optically absorptive anisotropic film may be colored.
[0069] <Optical film> FIG. 1 is a cross-sectional view showing a schematic diagram of an optical film according to one embodiment of the present invention. The optical film 10 has the above-described optically absorptive anisotropic film 11 and a first base layer (base layer) 12. The first base layer 12 may be a layer to which a composition for forming an optically absorptive anisotropic film is applied to form the optically absorptive anisotropic film 11, or may constitute a part of the layer. The first base layer 12 may have a single-layer structure or a multi-layer structure. The details of the first base layer 12 will be described later.
[0070] The optical film 10 may have the optically absorptive anisotropic film 11 and the first base layer 12 in direct contact with each other, or may have the above-mentioned first alignment layer between the optically absorptive anisotropic film 11 and the first base layer 12. When the optical film 10 has the first alignment layer, it is preferable that the first alignment layer is in direct contact with the optically absorptive anisotropic film 11 and the first base layer 12.
[0071] (1st base layer) The first substrate layer can support the optically absorptive anisotropic film. The first substrate layer may be a film substrate, a coating layer, a film with a coating layer formed on one or both sides of the film substrate, a film with a surface protective film laminated on the surface of the film substrate opposite to the optically absorptive anisotropic film side, or a resin layer such as a film with a coating layer formed on one surface of the film substrate and a surface protective film laminated on the other surface. The substrate layer may be a glass substrate. The substrate layer is preferably a resin layer.
[0072] Examples of resins that constitute the film substrate include olefin resins such as polyethylene and polypropylene; cyclic olefin resins having a cyclo- or norbornene structure; polyvinyl alcohol; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; poly(meth)acrylic resins; cellulose ester resins such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyimide resins; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide; polyphenylene oxide, etc.
[0073] The film substrate may be a commercially available cellulose ester resin film, such as "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.), "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.).
[0074] Commercially available cyclic olefin resins may be used as the cyclic olefin resin constituting the film substrate. Examples of such cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona (Germany)), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). These cyclic olefin resins can be made into a film substrate by forming a film by known means such as a solvent casting method or a melt extrusion method.
[0075] As the film substrate, a commercially available cyclic olefin resin substrate may be used. Examples of such cyclic olefin resin substrates include "S-Cina" (registered trademark), "SCA40" (registered trademark) (both manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "ARTON Film" (registered trademark) (manufactured by JSR Corporation).
[0076] When the first base layer is a coating layer, for example, the above-mentioned film with coating layer may be used, a light absorption anisotropic film may be formed on the film with coating layer, and the film base may be peeled off to obtain an optical film. Alternatively, the light absorption anisotropic film and an elliptically polarizing plate (described later) may be laminated before peeling off the film base, and then the film base may be peeled off. By performing a release treatment to form a release layer by applying a release agent or the like on the surface of the film base on which the coating layer is formed, the film base is easily peeled off. By peeling off the film base in this way, an optical film including a coating layer as the first base layer and a light absorption anisotropic film may be obtained.
[0077] Examples of the coating layer include a layer formed by applying a hard-coating agent, an easy-adhesion composition, or a coupling agent to the surface of a film substrate, and a layer formed by applying a reactive monomer or a reactive polymer to the surface of the film substrate and then graft-polymerizing the reactive monomer or polymer by irradiating the reactive monomer or polymer with active energy rays. As the film with a coating layer, a hard-coated film having a hard-coated layer as the coating layer is preferable. When the first substrate layer is a hard-coated film, it is preferable that a light-absorption anisotropic film is laminated on the hard-coated layer side. As the coating layer, a hard-coated layer is preferable.
[0078] The hard coat layer is preferably a cured product layer of a curable composition containing an active energy ray curable resin, and more preferably a cured product layer of a composition containing an ultraviolet ray curable resin. The curable composition containing an ultraviolet ray curable resin preferably contains a (meth)acrylic compound as a curable component, and the hard coat layer is preferably formed of a poly(meth)acrylic resin. The (meth)acrylic compound is a compound having at least one (meth)acryloyl group, and may be a monomer, oligomer, or polymer.
[0079] Examples of the (meth)acrylic compound include (meth)acrylate compounds such as monofunctional (meth)acrylate compounds and polyfunctional (meth)acrylate compounds; urethane (meth)acrylate compounds such as polyfunctional urethane (meth)acrylate compounds; epoxy (meth)acrylate compounds such as polyfunctional epoxy (meth)acrylate compounds; carboxyl group-modified epoxy (meth)acrylate compounds; polyester (meth)acrylate compounds, etc. These can be used alone or in combination. Among these, polyfunctional (meth)acrylate compounds or urethane (meth)acrylate compounds are preferred, and it is more preferred to combine a polyfunctional (meth)acrylate compound with a urethane (meth)acrylate.
[0080] The content of the polyfunctional (meth)acrylate compound is preferably 50 parts by mass or more and 100 parts by mass or less, more preferably 60 parts by mass or more and 95 parts by mass or less, and even more preferably 70 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the solid content of the curable composition. In this specification, the solid content of the curable composition refers to the total amount of components excluding the solvent from the curable composition when the curable composition contains a solvent.
[0081] The curable composition may contain a polymerization initiator in addition to the curable component. Examples of the polymerization initiator include a photopolymerization initiator and a radical polymerization initiator, and known polymerization initiators may be used.
[0082] The curable composition can be applied to a film substrate and then irradiated with active energy rays to polymerize the curable components such as the (meth)acrylic compound and cure the composition.
[0083] The hard coat layer preferably exhibits a value of 8B or harder in a pencil hardness test (measured by placing the film substrate on a glass plate) specified in JIS K 5600-5-4:1999 "General test methods for paints - Part 5: Mechanical properties of coatings - Section 4: Scratch hardness (pencil method)" and may exhibit a value of 5B or harder.
[0084] The surface protection film constituting the film with surface protection film is provided releasably on the film substrate constituting the first substrate layer. The surface protection film may have a multilayer structure of a resin film and an adhesive layer, or may be a self-adhesive film made of a resin film having a single layer structure. Examples of the resin film used in the surface protection film having a multilayer structure include films formed of the resins exemplified as the resins constituting the film substrate. Examples of the self-adhesive film include films using polypropylene-based resins and polyethylene-based resins. The surface protection film is usually removed after the light absorption anisotropic film is applied to a display device.
[0085] The surface of the first base layer on which the optically absorptive anisotropic film is formed may be subjected to a surface treatment. Examples of the surface treatment method include a method of subjecting the surface of the first base layer to corona treatment or plasma treatment under an atmosphere from vacuum to atmospheric pressure, a method of laser treatment, a method of ozone treatment, a method of flame treatment, a method of saponifying the surface of the first base layer, and the like.
[0086] The thickness of the first base layer is preferably thin in terms of the mass that can be practically handled, but if it is too thin, the strength decreases and the processability tends to be poor. From this viewpoint, the thickness of the first base layer is preferably 30 μm or more and 150 μm or less, may be 40 μm or more and 150 μm or less, may be 50 μm or more and 140 μm or less, may be 60 μm or more and 130 μm or less, or may be 70 μm or more and 120 μm or less.
[0087] (First alignment layer) The first alignment layer facilitates the alignment of the liquid crystal of the polymerizable liquid crystal compound. The state of the liquid crystal alignment varies depending on the properties of the first alignment layer and the polymerizable liquid crystal compound, and the combination can be selected arbitrarily. When the optical film has a first alignment layer, the first alignment layer may be formed on the surface of the first base layer on the side where the light absorption anisotropic film is formed.
[0088] When the first alignment layer is made of an alignment polymer, the alignment regulating force can be adjusted as desired by changing the surface state and rubbing conditions. When the first alignment layer is made of a photoalignment polymer, the alignment regulating force can be adjusted as desired by changing the polarized light irradiation conditions, etc. In addition, the liquid crystal alignment can be controlled by selecting the physical properties, such as the surface tension and liquid crystallinity, of the polymerizable liquid crystal compound.
[0089] The first alignment layer is preferably insoluble in a solvent used to form a light absorption anisotropic film on the first alignment layer, and has heat resistance to the heat treatment for removing the solvent and for orienting the liquid crystal. Examples of the first alignment layer include a polymer alignment layer made of an orientable polymer, a photoalignment layer, a groove alignment layer, and a stretched film stretched in the alignment direction. When applied to a long rolled film, a photoalignment layer is preferred because the alignment direction can be easily controlled.
[0090] The thickness of the first alignment layer is usually in the range of 10 nm to 5000 nm, preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 to 300 nm.
[0091] Examples of the alignment polymer used in the rubbing alignment layer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and their hydrolyzates, such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. These alignment polymers may be used alone or in combination of two or more.
[0092] An example of a rubbing method is to apply an oriented polymer composition to a layer constituting the first substrate layer, anneal the layer, and then contact the resulting oriented polymer film that constitutes the surface of the first substrate layer with a rotating rubbing roll wrapped with a rubbing cloth.
[0093] The photo-alignment layer is made of a polymer, oligomer, or monomer having a photoreactive group. The photo-alignment layer is obtained by irradiating a coating layer formed by applying a composition for forming a photo-alignment layer to a layer constituting the first base layer with polarized light. The photo-alignment layer is more preferable in that the direction of the alignment regulating force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0094] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of liquid crystal alignment ability, such as molecular alignment induction caused by irradiation with light, or an isomerization reaction, a dimerization reaction, a photocrosslinking reaction, or a photodecomposition reaction. Among the photoreactive groups, those that cause a dimerization reaction or a photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group that can generate the above-mentioned reaction, those having an unsaturated bond, particularly a double bond, are preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) are more preferred.
[0095] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. From the viewpoint of easy control of reactivity and expression of alignment control force during photoalignment, chalcone groups and cinnamoyl groups are preferred. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, and formazan groups, and groups having azoxybenzene as a basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0096] The polarized light may be irradiated directly from the film surface of the coating layer of the composition for forming the photo-alignment layer, or may be irradiated from the underlayer side such as the first base layer, and then transmitted through the film. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the above-mentioned light source can be irradiated through an appropriate polarizer to irradiate the polarized light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.
[0097] <Optical laminate> 2 is a cross-sectional view showing a schematic diagram of an optical laminate according to one embodiment of the present invention. The optical laminate 30 includes the above-mentioned light absorptive anisotropic film 11 or optical film 10, and an elliptically polarizing plate 20. The elliptically polarizing plate 20 may be an anti-reflection film.
[0098] In the optical laminate 30, the light absorptive anisotropic film 11 or the optical film 10 may be in direct contact with the elliptically polarizing plate 20, or may be laminated via a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer or an adhesive layer.
[0099] The light absorbing anisotropic film 11 or the optical film 10 is preferably provided on the polarizing element 21 side (viewing side) of the elliptical polarizer 20. The optical film 10 may have the light absorbing anisotropic film 11 side laminated thereon, or the first base layer 12 side laminated thereon, as shown in FIG. 2. By laminating the light absorbing anisotropic film 11 or the optical film 10 on the viewing side of the elliptical polarizer 20, when the optical laminate 30 is applied to a display device, the hue difference between the front hue when viewed from the front during white display and the oblique hue when viewed from an oblique direction can be reduced. In addition, as described above, when the display device to which the optical laminate 30 is applied is displayed in white and the display screen is viewed from an oblique direction, it is possible to suppress the visibility of white line-like unevenness.
[0100] (Elliptical polarizing plate) The elliptical polarizer 20 may have, in order from the viewing side, a polarizing element 21 and a first phase difference element 22 having an in-plane phase difference. The first phase difference element 22 may include two or more layers of phase difference elements having different in-plane phase differences. In order to highly achieve the anti-reflection function of the elliptical polarizer 20 as an anti-reflection film, it is preferable to include a λ / 4 phase difference element having a λ / 4 plate function (i.e., a π / 2 phase difference function) in the entire visible light range. The λ / 4 phase difference element is preferably a λ / 4 phase difference element with reverse wavelength dispersion. The first phase difference element 22 may be a combination of a phase difference element (λ / 2 phase difference element) having a λ / 2 plate function with positive wavelength dispersion and a λ / 4 phase difference element with positive wavelength dispersion.
[0101] The elliptically polarizing plate 20 may further include a second phase difference element 23 (positive C plate) having anisotropy in the thickness direction, from the viewpoint of being able to compensate for the anti-reflection function in oblique directions.
[0102] When the retardation element constituting the first retardation element 22 and the second retardation element 23 are liquid crystal retardation layers obtained from a composition containing a polymerizable liquid crystal compound, these liquid crystal retardation layers may independently form a tilt alignment state or a cholesteric alignment state.
[0103] When the elliptical polarizer 20 includes the first phase difference element 22 and the second phase difference element 23, the elliptical polarizer 20 in the optical laminate 30 may have, from the light absorption anisotropic film 11 side, a polarizer 21, a first phase difference element 22, and a second phase difference element 23 in this order, or may have the polarizer 21, the second phase difference element 23, and the first phase difference element 22 in this order. A pressure-sensitive adhesive layer may be provided between the layers constituting the elliptical polarizer 20.
[0104] The polarizing element 21 included in the elliptical polarizing plate 20 has light absorption anisotropy. The polarizing element 21 will be described in detail later, but the polarizing element 21 is, for example, a layer in which a dichroic dye, which is a dye having light absorption anisotropy, is uniaxially oriented. Examples of the polarizing element in which the dichroic dye is uniaxially oriented include a polarizer formed by uniaxially stretching a polymer such as a polyvinyl alcohol resin in a state in which iodine or an organic dichroic dye is impregnated; and a liquid crystal polarizer made of a polymer of a polymerizable liquid crystal compound containing a dichroic dye, which is formed by orienting a dichroic dye and a polymerizable liquid crystal compound from a composition containing a polymerizable liquid crystal compound and a dichroic dye. Such a polarizing element can exhibit a polarizing function by anisotropically absorbing light by the dichroic dye included in the stretched film or the polymer of the polymerizable liquid crystal compound. The polarizing element 21 may be incorporated into the optical laminate 30 after being made into a polarizing plate in which a polarizing element protective film is laminated on one or both sides. The polarizing plate will be described in detail later.
[0105] It is preferable that the in-plane retardation R(λ) of the first retardation element 22 included in the elliptical polarizing plate 20 for light of wavelength λ [nm] satisfies the optical characteristics shown in the following formula (3), and it is preferable that the optical characteristics satisfies the following formulas (3), (4), and (5). 100nm <Re(550)<160nm (3) Re(450) / Re(550)≦1.00 (4) 1.00≦Re(650) / Re(550) (5) [In formulas (3) to (5), Re(550) represents the in-plane retardation value (in-plane retardation) of the first retardation element for light with a wavelength of 550 nm, Re(450) represents the in-plane retardation value of the first retardation element for light having a wavelength of 450 nm, Re(650) represents the in-plane retardation value of the first retardation element for light with a wavelength of 650 nm.]
[0106] When "Re(450) / Re(550)" in the above formula (4) exceeds 1.0, the light leakage on the short wavelength side of the elliptical polarizer 20 having a λ / 4 retardation element becomes large. "Re(450) / Re(550)" is preferably 0.70 or more and 1.00 or less, more preferably 0.80 or more and 0.95 or less, even more preferably 0.80 or more and 0.92 or less, and particularly preferably 0.82 or more and 0.88 or less. The value of "Re(450) / Re(550)" can be arbitrarily adjusted by adjusting the stacking angle and retardation value of the multiple retardation elements constituting the first retardation element 22, or by adjusting the mixing ratio of the polymerizable liquid crystal compound constituting the first retardation element 22.
[0107] The in-plane retardation value of the first retardation element 22 and the retardation element constituting the first retardation element 22 can be adjusted by the thickness of these layers. Since the in-plane retardation value is determined by the following formula (6), in order to set the in-plane retardation value (Re(λ)) at a wavelength λ [nm] to a desired value, Δn(λ) and the film thickness d may be adjusted. The thickness of the first retardation element 22 and the retardation element constituting the first retardation element 22 is preferably 0.5 μm to 5 μm, more preferably 1 μm to 3 μm, independently of each other. The thickness can be measured by an interference film thickness meter, a laser microscope, or a stylus film thickness meter. In addition, when the first retardation element 22 is a first liquid crystal retardation layer formed using a polymerizable liquid crystal compound, Δn(λ) depends on the molecular structure of the polymerizable liquid crystal compound. Re(λ)=d×Δn(λ) (6) [In formula (6), Re(λ) represents the in-plane retardation value of the retardation element at a wavelength λ [nm], d represents the thickness of the phase difference element, Δn(λ) represents the birefringence of the retardation element at a wavelength λ [nm].
[0108] The second retardation element 23 included in the elliptically polarizing plate 20 is preferably a positive C plate. The retardation value Rth(550) in the thickness direction at a wavelength of 550 nm of the positive C plate is usually in the range of -170 nm or more and -10 nm or less, preferably in the range of -150 nm or more and -20 nm or less, and more preferably in the range of -100 nm or more and -40 nm or less. If the retardation value in the thickness direction of the positive C plate is in this range, the anti-reflection property from an oblique direction can be further improved.
[0109] When the first retardation element 22 and the second retardation element 23 are liquid crystal retardation layers obtained by polymerizing a polymerizable liquid crystal compound, the first liquid crystal retardation layer (first retardation element 22) and the second liquid crystal retardation layer (second retardation element 23) may be incorporated into the optical laminate 30 in a state where they are laminated with a third base layer (described later) that supports them. In this case, the liquid crystal retardation layer constituting the first liquid crystal retardation layer can be in direct contact with the third base layer, and the second liquid crystal retardation layer can be in direct contact with the third base layer.
[0110] Each layer constituting the elliptically polarizing plate will now be described in detail. (Polarizing element) When unpolarized light is incident on a polarizing element, it has the property of transmitting linearly polarized light whose vibration plane is perpendicular to the absorption axis. Polarizing elements have an absorption axis and a transmission axis perpendicular to the absorption axis in their plane, and have the property of absorbing polarized components parallel to the absorption axis and transmitting polarized components parallel to the transmission axis.
[0111] The polarizing element may be a polarizer which is a stretched polarizing film in which a dye having absorption anisotropy is adsorbed onto a polymer such as a polyvinyl alcohol-based resin (hereinafter, a stretched polarizing film using a polyvinyl alcohol-based resin as the polymer may be referred to as a "PVA polarizer"); or a liquid crystal polarizer which includes a liquid crystal cured film formed by applying a liquid crystal polarizer-forming composition containing a dye having absorption anisotropy and a compound having liquid crystal properties to a second substrate layer. An example of the dye having absorption anisotropy is a dichroic dye. The dichroic dye contained in the PVA polarizer is preferably iodine.
[0112] A PVA polarizer can be obtained through a process including a step of uniaxially stretching a polyvinyl alcohol-based resin film (hereinafter sometimes referred to as a "PVA-based film"), a step of dyeing the PVA-based film with a dichroic dye to adsorb the dichroic dye, a step of treating the PVA-based film with the adsorbed dichroic dye with an aqueous boric acid solution, and, if necessary, a step of washing with water after the treatment with the aqueous boric acid solution.
[0113] The thickness of the PVA polarizer is usually 30 μm or less, preferably 18 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less. The thickness is usually 1 μm or more, for example, 5 μm or more.
[0114] The uniaxial stretching of the PVA-based film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. Of course, the uniaxial stretching can be performed in the multiple stages shown here. For the uniaxial stretching, a method of uniaxially stretching in the film transport direction between rolls having different peripheral speeds, a method of uniaxially stretching in the film transport direction using a heated roll, a method of stretching in the width direction using a tenter, etc. can be adopted. The uniaxial stretching may be performed by dry stretching in the air, or by wet stretching in a state in which the PVA-based film is swollen using a solvent such as water. The stretching ratio is usually about 3 to 8 times. In addition, an aqueous solution containing polyvinyl alcohol may be applied to the thermoplastic resin film, followed by drying treatment, and stretched together with the thermoplastic resin film by the above method.
[0115] The dyeing of the PVA-based film with a dichroic dye can be carried out, for example, by immersing the PVA-based film in an aqueous solution containing the dichroic dye. Specifically, iodine or a dichroic organic dye is used as the dichroic dye.
[0116] A liquid crystal polarizer formed from a composition for forming a liquid crystal polarizer, which contains a dye having absorption anisotropy and a polymerizable liquid crystal compound, can be suitably used for, for example, flexible display applications, since the hue can be arbitrarily controlled, the thickness can be significantly reduced, and the polarizer is non-shrinkable since it is not stretched or relaxed by heat.
[0117] The liquid crystal polarizer includes a liquid crystal cured film obtained by, for example, applying a composition for forming a liquid crystal polarizer onto a second substrate layer, and polymerizing a polymerizable liquid crystal compound in a state in which a dichroic dye contained in the composition for forming a liquid crystal polarizer is aligned. The liquid crystal polarizer may be a liquid crystal cured film, or may be a laminate of the liquid crystal cured film and a second alignment layer. The dichroic dye and the polymer of the polymerizable liquid crystal compound contained in the liquid crystal polarizer are aligned horizontally with respect to the surface of the second substrate layer.
[0118] The thickness of the liquid crystal cured film included in the liquid crystal polarizer is preferably 0.1 μm to 5 μm, more preferably 0.3 μm to 4 μm, and even more preferably 0.5 μm to 3 μm. If the thickness is smaller than this range, the necessary light absorption may not be obtained, and if the thickness is larger than this range, the alignment control force by the second alignment layer decreases, and alignment defects tend to occur easily.
[0119] The liquid crystal polarizer preferably has a ratio (dichroic ratio; A1 / A2) of absorbance A1(λ) in the alignment direction for light of wavelength λ [nm] to absorbance A2(λ) in the direction perpendicular to the in-plane alignment direction of the liquid crystal polarizer, which is 7 or more, more preferably 20 or more, and further preferably 40 or more. It can be said that the larger the dichroic ratio, the better the absorption selectivity. Although it depends on the type of dichroic dye, when the liquid crystal cured film contained in the liquid crystal polarizer is cured in a nematic liquid crystal phase state, the dichroic ratio is about 5 to 10.
[0120] By mixing two or more dichroic dyes with different absorption wavelengths, it is possible to produce liquid crystal polarizers with various hues, and liquid crystal polarizers with absorption over the entire visible light range can be produced. Liquid crystal polarizers with such absorption characteristics can be used in a variety of applications.
[0121] The second substrate layer may be one described as the first substrate layer of the optical film. The second substrate layer may be peeled off when forming an anti-reflection film, but may not be peeled off and may be used as a polarizing element protective film of a liquid crystal polarizer. The dichroic dye used in the liquid crystal polarizer may be the dichroic dye used in the light absorption anisotropic film. The polymerizable liquid crystal compound may be a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or a mixture thereof. The polymerizable liquid crystal compound may be a thermotropic liquid crystal compound exhibiting a nematic liquid crystal phase, or a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase. The compound having liquid crystal properties and the polymerizable liquid crystal compound may be the polymerizable liquid crystal compound used in the light absorption anisotropic film.
[0122] The second alignment layer that may be included in the liquid crystal polarizer is preferably a horizontal alignment layer that can align the polymerizable liquid crystal compound in a direction horizontal to the surface of the liquid crystal polarizer. Examples of the second alignment layer include a polymer alignment layer formed of an alignment polymer, a photoalignment layer formed of a photoalignment polymer, and a groove alignment layer having a concave-convex pattern or a plurality of grooves on the layer surface. From the viewpoint of the precision and quality of the alignment angle, the second alignment layer is preferably a photoalignment layer. Examples of the above-mentioned alignment layers that constitute the second alignment layer include those described for the first alignment layer.
[0123] (Polarizing plate) The polarizing plate is a linear polarizing plate having a polarizing element protective film on one or both sides of the polarizing element. The polarizing element protective film is a resin film laminated on the polarizing element via a pressure-sensitive adhesive layer, and is a resin film that cannot be peeled off while maintaining the shape of the polarizing element. A thermoplastic resin film can be used as the polarizing element protective film. The thermoplastic resin film may be surface-treated (e.g., corona treatment, etc.) to improve adhesion to the polarizing element, and a thin layer such as a primer layer (also called an undercoat layer) may be formed.
[0124] The thermoplastic resin constituting the thermoplastic resin film is preferably a transparent film, and examples thereof include cellulose resins such as triacetyl cellulose; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyethersulfone resins; polysulfone resins; polycarbonate resins; polyamide resins such as nylon and aromatic polyamide; polyimide resins; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; cyclic polyolefin resins having cyclo- and norbornene structures (also called norbornene-based resins); (meth)acrylic resins; polyarylate resins; polystyrene resins; polyvinyl alcohol resins, etc. Among these, the thermoplastic resin film is preferably a cyclic polyolefin-based resin film, a cellulose ester-based resin film, a polyester-based resin film, or a (meth)acrylic resin film.
[0125] The polarizing element protective film may be one in which a hard coat layer is formed on a thermoplastic resin film. The hard coat layer may be formed on one side of the thermoplastic resin film, or on both sides. By providing the hard coat layer, the thermoplastic resin film can be improved in hardness and scratch resistance. The hard coat layer is, for example, a cured layer of an active energy ray curable resin, preferably an ultraviolet ray curable resin. Examples of the ultraviolet ray curable resin include poly(meth)acrylic resin, silicone resin, polyester resin, urethane resin, amide resin, and epoxy resin. The hard coat layer may contain an additive to improve strength. The additive is not particularly limited, and examples thereof include inorganic fine particles, organic fine particles, and mixtures thereof.
[0126] The thickness of the polarizing element protective film is preferably from 5 μm to 150 μm, and may be from 10 μm to 100 μm, or may be from 10 μm to 80 μm.
[0127] (First phase difference element, second phase difference element) The first retardation element and the second retardation element (hereinafter, these may be collectively referred to as "retardation elements") may be a retardation layer which is a stretched film, or may be a liquid crystal retardation layer containing a polymer of a polymerizable liquid crystal compound, but is preferably a liquid crystal retardation layer.
[0128] The retardation layer may be a conventionally known one, and may be a resin film that is uniaxially or biaxially stretched to give a retardation. As the resin film, cellulose films such as triacetyl cellulose and diacetyl cellulose, polyester films such as polyethylene terephthalate, polyethylene isophthalate and polybutylene terephthalate, acrylic resin films such as polymethyl (meth) acrylate and polyethyl (meth) acrylate, polycarbonate films, polyethersulfone films, polysulfone films, polyimide films, polyolefin films, polynorbornene films, etc. may be used, but are not limited thereto.
[0129] The thickness of the retardation layer is usually from 5 μm to 200 μm, preferably from 10 μm to 80 μm, and more preferably from 40 μm to 50 μm.
[0130] When the retardation element is a liquid crystal retardation layer, the liquid crystal retardation layer may include a liquid crystal cured film formed by applying a liquid crystal retardation layer forming composition containing a polymerizable liquid crystal compound to a third base layer. The liquid crystal retardation layer may be a liquid crystal cured film or a laminate of a liquid crystal cured film and a third alignment layer. The liquid crystal retardation layer exhibits retardation in the in-plane direction or thickness direction.
[0131] Examples of the third substrate layer include those described for the first substrate layer. The third substrate layer may be peeled off when forming an anti-reflection film, but may be used as a protective film for the liquid crystal retardation layer without peeling off. The polymerizable liquid crystal compound may be a polymerizable liquid crystal compound having a photopolymerizable group as a polymerizable group. For example, a polymerizable liquid crystal compound conventionally known in the field of liquid crystal retardation layers may be used as the polymerizable liquid crystal compound. The photopolymerizable group refers to a group that can participate in a polymerization reaction by a reactive species generated from a photopolymerization initiator, such as an active radical or an acid. Examples of the photopolymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred. The liquid crystal may be either thermotropic or lyotropic, but thermotropic liquid crystal is preferred because it allows precise control of the film thickness. The phase ordered structure in the thermotropic liquid crystal may be either nematic or smectic. The phase ordered structure may be either rod-shaped or discotic. The polymerizable liquid crystal compound may be used alone or in combination of two or more kinds.
[0132] As the polymerizable liquid crystal compound contained in the λ / 4 liquid crystal retardation layer contained in the first liquid crystal retardation layer, a liquid crystal having a T-shaped or H-shaped mesogen structure further having birefringence in a direction perpendicular to the molecular long axis direction is preferable from the viewpoint of expressing reverse wavelength dispersion, and a T-shaped liquid crystal is more preferable from the viewpoint of obtaining stronger dispersion. Specific examples of the T-shaped liquid crystal structure include a compound represented by the following formula (d). [ka] [In formula (d), Ar represents a divalent aromatic group which may have a substituent. The divalent aromatic group preferably contains at least one of a nitrogen atom, an oxygen atom, and a sulfur atom. When the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other via a divalent bonding group such as a single bond, -CO-O-, or -O-. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. L 1 , L 2 , B 1 and B. 2 each independently represents a single bond or a divalent linking group. k and l each independently represent an integer of 0 to 3, and satisfy the relationship of 1≦k+l. Here, when 2≦k+l, B 1 and B. 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms, in which a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and -CH2- contained in the alkanediyl group may be substituted with -O-, -S- or -COO-, and when there are a plurality of -O-, -S- or -COO-, they are not adjacent to each other. P 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
[0133] G 1 and G 2are each independently preferably a 1,4-phenylenediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, more preferably a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group. In addition, there are multiple G 1 and G 2 At least one of L is preferably a divalent alicyclic hydrocarbon group. 1 Or L 2 G binds to 1 and G 2 It is more preferable that at least one of the groups is a divalent alicyclic hydrocarbon group.
[0134] L 1 and L 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -, -R a3 COOR a4 -, -R a5 O.C.O.R. a6 -, R a7 OC=OOR a8 -, -N=N-, -CR c =CR d -, or C≡C-, where R a1 ~R a8 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms; R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 are each independently preferably a single bond, -O Ra2-1 -, -CH2-, -CH2CH2-, -COOR a4-1 - or OCORa6-1 -, where R a2-1 , R a4-1 , R a6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 are each independently more preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or OCO-.
[0135] B 1 and B. 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -, -R a11 COOR a12 -, -R a13 OCOR a14 - or R a15 OC=OOR a16 -, where R a9 ~R a16 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B. 2 are each independently preferably a single bond, -OR a10-1 -, -CH2-, -CH2CH2-, -COOR a12-1 - or OCOR a14-1 -, where R a10-1 , R a12-1 , R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. B 1 and B. 2 are each independently more preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or OCOCH2CH2-.
[0136] From the viewpoint of expressing reverse wavelength dispersion, k and l are preferably in the range of 2≦k+l≦6, preferably k+l=4, and more preferably k=2 and l=2. When k=2 and l=2, a symmetrical structure is obtained, which is preferable.
[0137] E1 and E 2 are each independently preferably an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms.
[0138] P 1 Or P 2 Examples of the polymerizable group represented by the formula (I) include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred.
[0139] It is preferable that Ar has at least one selected from an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, and an electron-withdrawing group. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring, and the like, and the benzene ring and the naphthalene ring are preferable. Examples of the aromatic heterocycle include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring. Among them, it is preferable that Ar has a thiazole ring, a benzothiazole ring, or a benzofuran ring, and it is more preferable that Ar has a benzothiazole group. In addition, when Ar contains a nitrogen atom, it is preferable that the nitrogen atom has a π electron.
[0140] In formula (d), the total number Nπ of π electrons contained in the divalent aromatic group represented by Ar is preferably 8 or more, more preferably 10 or more, even more preferably 14 or more, and particularly preferably 16 or more. Also, it is preferably 30 or less, more preferably 26 or less, and even more preferably 24 or less.
[0141] Suitable examples of the aromatic group represented by Ar include the following groups: [ka] [Formula (Ar-1) to formula (Ar-23), * indicates the connection part. Z 0 , Z 1 and Z 2 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms. Q 1 and Q 2 are each independently -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ represents -, -CO- or O-; R 2 ' and R 3’ each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. J 1 , and J 2 each independently represents a carbon atom or a nitrogen atom. Y 1 , Y 2 and Y 3 each independently represents an optionally substituted aromatic hydrocarbon group or an optionally substituted aromatic heterocyclic group. W 1 and W 2 each independently represents a hydrogen atom, a cyano group, a methyl group, or a halogen atom. m represents an integer from 0 to 6.
[0142] Y 1 , Y 2 and Y3 Examples of the aromatic hydrocarbon group in the formula (I) include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a biphenyl group, of which a phenyl group and a naphthyl group are preferred, and a phenyl group is more preferred. Examples of the aromatic heterocyclic group in the formula (I) include aromatic heterocyclic groups having 4 to 20 carbon atoms and containing at least one heteroatom, such as a nitrogen atom, an oxygen atom, or a sulfur atom, such as a furyl group, a pyrrolyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group, of which a furyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group are preferred.
[0143] Y 1 , Y 2 and Y 3 may each independently be an optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.
[0144] Z 0 , Z 1 and Z 2 are each preferably independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms; Z 0 is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group; Z 1 and Z 2 is more preferably a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group.
[0145] Q 1 and Q 2 -NH-, -S-, -NR 2’ -, -O- are preferred, R 2’ is preferably a hydrogen atom, and among these, -S-, -O-, and -NH- are particularly preferable.
[0146] Among the compounds represented by formulae (Ar-1) to (Ar-23), the compounds represented by formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.
[0147] In the compounds represented by formulae (Ar-16) to (Ar-23), Y 1 is the nitrogen atom to which it is bonded and Z 0 and may form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those mentioned above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. This aromatic heterocyclic group may have a substituent. In addition, Y 1 is the nitrogen atom to which it is bonded and Z 0 In addition, it may be the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc.
[0148] Among the polymerizable liquid crystal compounds, compounds having a maximum absorption wavelength of 300 to 400 nm are preferred. When a photopolymerization initiator is contained in a liquid crystal retardation layer forming composition containing a polymerizable liquid crystal compound, the polymerization reaction and gelation of the polymerizable liquid crystal compound may proceed during long-term storage. However, if the maximum absorption wavelength of the polymerizable liquid crystal compound is 300 to 400 nm, even if the composition is exposed to ultraviolet light during storage, the generation of reactive species from the photopolymerization initiator and the polymerization reaction and gelation of the polymerizable liquid crystal compound caused by the reactive species can be effectively suppressed. Therefore, it is advantageous in terms of long-term stability of the liquid crystal retardation layer forming composition, and the alignment property and thickness uniformity of the liquid crystal cured film contained in the first liquid crystal retardation layer can be improved. The maximum absorption wavelength of the polymerizable liquid crystal compound can be measured using an ultraviolet-visible spectrophotometer in a solvent. The solvent is a solvent that can dissolve the polymerizable liquid crystal compound, and examples thereof include chloroform and the like.
[0149] The content of the polymerizable liquid crystal compound in the liquid crystal retardation layer forming composition is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass, based on 100 parts by mass of the solid content of the liquid crystal retardation layer forming composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the viewpoint of the alignment of the obtained liquid crystal cured film.
[0150] The liquid crystal retardation layer may include a third alignment layer. The third alignment layer may be selected according to the direction in which the polymerizable liquid crystal compound is aligned, and may be a vertical alignment layer or a horizontal alignment layer. If the third alignment layer is a material that exhibits horizontal alignment as an alignment regulating force, the polymerizable liquid crystal compound can form a horizontal alignment or a hybrid alignment, and if the third alignment layer is a material that exhibits vertical alignment, the polymerizable liquid crystal compound can form a vertical alignment or an inclined alignment. The expressions horizontal, vertical, and the like represent the direction of the long axis of the aligned polymerizable liquid crystal compound when the plane of the first liquid crystal retardation layer or the second liquid crystal retardation layer is used as a reference. For example, vertical alignment means that the long axis of the aligned polymerizable liquid crystal compound is aligned in a direction perpendicular to the plane of the first liquid crystal retardation layer or the second liquid crystal retardation layer. Here, horizontal means 0°±20° with respect to the plane of the first liquid crystal retardation layer or the second liquid crystal retardation layer, and vertical means 90°±20° with respect to the plane of the first liquid crystal retardation layer or the second liquid crystal retardation layer. As the third alignment layer, those described for the first alignment layer and the second alignment layer can be mentioned.
[0151] The thickness of the liquid crystal retardation layer is preferably 0.5 μm or more and 5 μm or less, and more preferably 1 μm or more and 3 μm or less.
[0152] (Adhesive layer) The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer or an adhesive layer.
[0153] The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition or the reaction product of the pressure-sensitive adhesive composition exhibits adhesiveness by attaching itself to an adherend, and is called a pressure-sensitive adhesive. In addition, the pressure-sensitive adhesive layer formed using the active energy ray curable pressure-sensitive adhesive composition described later can be irradiated with active energy rays to adjust the crosslinking degree and adhesive strength.
[0154] As the adhesive composition, a conventionally known adhesive having excellent optical transparency can be used without any particular limitation, and for example, an adhesive composition containing a base polymer such as an acrylic polymer, a urethane polymer, a silicone polymer, or a polyvinyl ether can be used. The adhesive composition may be an active energy ray curable adhesive composition or a heat curable adhesive composition. Among these, an adhesive composition using an acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, removability (reworkability), weather resistance, heat resistance, etc., is preferable. The adhesive layer is preferably composed of a reaction product of an adhesive composition containing a (meth)acrylic resin, a crosslinking agent, and a silane compound, and may contain other components.
[0155] The adhesive composition for forming the adhesive layer may contain a base polymer such as an acrylic polymer, a urethane polymer, a silicone polymer, or a polyvinyl ether. The adhesive composition may be an active energy ray curable adhesive, a heat curable adhesive, or the like. Among these, an adhesive having a (meth)acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, removability (reworkability), weather resistance, heat resistance, and the like, is preferred. The adhesive layer is preferably composed of a reaction product of an adhesive containing a (meth)acrylic resin, a crosslinking agent, and a silane compound, and may contain other components.
[0156] The adhesive layer may be formed using an active energy ray curable adhesive. The active energy ray curable adhesive is prepared by blending an ultraviolet curable compound such as a multifunctional acrylate with the above-mentioned adhesive composition, forming an adhesive layer, and then curing the adhesive layer by irradiating it with ultraviolet light, thereby forming a harder adhesive layer. The active energy ray curable adhesive has a property of being cured by irradiation with energy rays such as ultraviolet rays and electron beams. The active energy ray curable adhesive has adhesiveness even before irradiation with energy rays, and therefore has a property of being able to adhere to an adherend and to be cured by irradiation with energy rays to adjust the adhesion.
[0157] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is usually from 5 μm to 300 μm, optionally from 10 μm to 250 μm, optionally from 15 μm to 100 μm, or optionally from 20 μm to 50 μm.
[0158] The adhesive layer can be formed using an adhesive composition. The adhesive composition for forming the adhesive layer is an adhesive other than a pressure-sensitive adhesive (adhesive), and examples thereof include a water-based adhesive and an active energy ray-curable adhesive.
[0159] Examples of the water-based adhesive include an adhesive in which a polyvinyl alcohol resin is dissolved or dispersed in water. The drying method when using a water-based adhesive is not particularly limited, but for example, a method of drying using a hot air dryer or an infrared dryer can be adopted.
[0160] Examples of the active energy ray curable adhesive include a solventless active energy ray curable adhesive containing a curable compound that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. By using a solventless active energy ray curable adhesive, the adhesion between layers can be improved.
[0161] The thickness of the adhesive layer is preferably 0.1 μm or more, and may be 0.5 μm or more, and is preferably 10 μm or less, and may be 5 μm or less.
[0162] <Display device> The above-mentioned light absorbing anisotropic film, optical film, or optical laminate can be applied to a display device. An example of the display device is an organic EL display device. The organic EL display device can have a structure in which the above-mentioned optical laminate is laminated on an image display element via a pressure-sensitive adhesive layer. In the organic EL display device, the optical laminate is incorporated so that the light absorbing anisotropic film, the elliptically polarizing plate, and the image display element are arranged in this order from the viewing side. The pressure-sensitive adhesive layer can be the pressure-sensitive adhesive layer described above. EXAMPLES
[0163] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. "%" and "parts" in the examples and comparative examples are by mass % and parts by mass unless otherwise specified.
[0164] Example 1 (Preparation of Optically Absorbent Anisotropic Film-Forming Composition (1)) The components shown below were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (1). Polymerizable liquid crystal compound (1): 75 parts Polymerizable liquid crystal compound (2): 25 parts Dichroic dye (1): 1 part Polymerization initiator (Irgacure 369, manufactured by BASF): 6 parts Leveling agent (F-556, manufactured by DIC): 0.25 parts Solvent (o-xylene): 300 parts
[0165] The polymerizable liquid crystal compounds (1) and (2) have the structures shown below and were synthesized according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). ·Polymerizable liquid crystal compound (1) (first liquid crystal compound): [ka] ·Polymerizable liquid crystal compound (2) (second liquid crystal compound): [ka]
[0166] The dichroic dye (1) used was an azo-based dye having the following structure and described in the Examples of JP 2013-101328 A. The maximum absorption wavelength of the dichroic dye (1) measured in a chloroform solution was 600 nm. Dichroic dyes (1): [ka]
[0167] (Preparation of Optical Film (1)) A triacetyl cellulose (TAC) film (KC8UX2M, manufactured by Konica Minolta, Inc.) was subjected to a corona treatment once using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min, and the film was cut out to form a first base layer (1). A light absorption anisotropic film-forming composition (1) was applied to the corona-treated surface of the first base layer (1) using a bar coater, and then dried for 1 minute in a drying oven set at a temperature of 100°C. Next, ultraviolet light was irradiated using a high-pressure mercury lamp (Uniqure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 500 mJ / cm2). 2 ) to form an optically absorptive anisotropic film (1) in which the polymerizable liquid crystal compound and the dichroic dye are aligned perpendicular to the coating plane. This resulted in an optical film (1) having a layer structure of the first base layer (1) / optically absorptive anisotropic film (1).
[0168] [Examples 2 and 3] Optically absorptive anisotropic film-forming compositions (2) and (3) were prepared in the same manner as in Example 1, except that the mixing ratio of the polymerizable liquid crystal compounds (1) and (2) was changed as shown in Table 1. Optically absorptive anisotropic film-forming compositions (2) and (3) were prepared using these compositions, and optically absorptive anisotropic films (2) and (3), respectively, were obtained.
[0169] Example 4 A composition for forming an optically absorptive anisotropic film (4) was prepared in the same manner as in Example 1, except that a polymerizable liquid crystal compound (3) having the structure shown below was used instead of the polymerizable liquid crystal compound (2). The composition was used to obtain an optically absorptive anisotropic film (4). ·Polymerizable liquid crystal compound (3) (second liquid crystal compound) [ka]
[0170] Example 5 A composition for forming an optically absorptive anisotropic film (5) was prepared in the same manner as in Example 1, except that 2.0 parts of dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester A-DPH") was added as a non-liquid crystal compound having a reactive group, and an optically absorptive anisotropic film (5) was obtained using this composition.
[0171] Example 6 An optical film (6) having an optically absorptive anisotropic film (6) was obtained in the same manner as in Example 5, except that the thickness of the optically absorptive anisotropic film was changed to the thickness shown in Table 1.
[0172] Comparative Example 1 A composition for forming an optically absorptive anisotropic film (c1) was prepared in the same manner as in Example 1, except that a polymerizable liquid crystal compound (4) having the structure shown below was used instead of the polymerizable liquid crystal compound (2), and an optical film (c1) having an optically absorptive anisotropic film (c1) was obtained using the composition. The polymerizable liquid crystal compound (4) is a polymerizable liquid crystal compound other than the first liquid crystal compound and the second liquid crystal compound. Polymerizable liquid crystal compounds (4) (other polymerizable liquid crystal compounds) [ka]
[0173] Comparative Example 2 A composition (c2) for forming an optically absorptive anisotropic film was prepared in the same manner as in Comparative Example 1, except that the mixing ratio of the polymerizable liquid crystal compounds (1) and (4) was changed as shown in Table 2, and an optically absorptive anisotropic film (c2) was obtained using the composition.
[0174] Comparative Example 3 A composition for forming an optically absorptive anisotropic film (c3) was prepared in the same manner as in Comparative Example 1, except that 2.0 parts of dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester A-DPH") was added as a non-liquid crystal compound having a reactive group, and an optically absorptive anisotropic film (c3) was obtained using this composition.
[0175] Comparative Example 4 A composition for forming an optically absorptive anisotropic film (c4) was prepared in the same manner as in Comparative Example 2, except that 2.0 parts of dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester A-DPH") was added as a non-liquid crystal compound having a reactive group, and an optically absorptive anisotropic film (c4) was obtained using this composition.
[0176] [Reference example 1] A composition for forming an optically absorptive anisotropic film (r1) was prepared in the same manner as in Comparative Example 2, except that the polymerizable liquid crystal compound (4) was replaced with a polymerizable liquid crystal compound (5) having the structure shown below, and the mixing ratio of the polymerizable liquid crystal compounds (1) and (5) was changed as shown in Table 2. The composition was used to obtain an optically absorptive anisotropic film (r1). The polymerizable liquid crystal compound (5) is a polymerizable liquid crystal compound exhibiting a nematic liquid crystal phase, and is a polymerizable liquid crystal compound other than the first liquid crystal compound and the second liquid crystal compound. Polymerizable liquid crystal compounds (5) (other polymerizable liquid crystal compounds) [ka]
[0177] [Reference example 2] (Preparation of composition for forming photoalignment layer) The following components described in JP2013-033249A were mixed, and the resulting mixture was stirred at 80°C for 1 hour to obtain a composition for forming a photoalignment layer. Photo-alignable polymer having the structure shown below: 2 parts [ka] Solvent (o-xylene): 98 parts
[0178] (Preparation of photo-alignment layer) A triacetyl cellulose (TAC) film (KC8UX2M, manufactured by Konica Minolta, Inc.) was used as the first base layer, and the film surface was subjected to a corona treatment, after which the composition for forming a photo-alignment layer was applied and dried at a temperature of 120°C to obtain a dry coating. Polarized UV was irradiated onto this dry coating to form a photo-alignment layer, thereby obtaining a first base layer with a photo-alignment layer. The polarized UV treatment was carried out using a UV irradiation device (SPOT CURE SP-7, manufactured by Ushio Inc.) under the condition of an intensity of 100 mJ measured at a wavelength of 365 nm.
[0179] (Preparation of liquid crystal polarizer (r2)) The composition for forming an optically absorbing anisotropic film (c1) prepared in Comparative Example 1 was applied onto the optical alignment layer of the first base layer with an optical alignment layer by a bar coating method (#9 30 mm / s), and the polymerizable liquid crystal compound was phase-transferred to a liquid phase by heating and drying in a drying oven at a temperature of 120°C for 1 minute, and then cooled to room temperature to cause the polymerizable liquid crystal compound to phase-transfer to a smectic liquid crystal state. Next, a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) was used to expose the polymerizable liquid crystal compound to a smectic liquid crystal state at an exposure dose of 1000 mJ / cm. 2By irradiating the layer formed from the light absorption anisotropic film-forming composition (c1) with ultraviolet light (365 nm standard), the polymerizable liquid crystal compound contained in the dried film was polymerized while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, forming a horizontally aligned liquid crystal polarizer (r2). As a result, an optical film (r1) having a layer structure of a first base layer / photo-alignment layer / liquid crystal polarizer was obtained.
[0180] [Reference example 3] A liquid crystal polarizer (r3) was formed and an optical film (r3) was obtained in the same manner as in Reference Example 2, except that the composition for forming an optically absorptive anisotropic film (c3) prepared in Comparative Example 3 was used instead of the composition for forming an optically absorptive anisotropic film (c1).
[0181] [Measurement of absorbance] The optical film was attached to a 4 cm x 4 cm x 0.7 mm thick glass plate via a 25 μm thick pressure-sensitive adhesive (manufactured by Lintec Corporation) to prepare a measurement sample (1). The sample was set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation's "UV-2450") to measure the absorbance, and Ax and Ax (z = 50) were determined. Since the absorbance of the first base layer can be regarded as 0 (zero), the Ax and Ax (z = 50) measured for the measurement sample (1) can be said to be the absorbance of the optically absorptive anisotropic film. The results are shown in Tables 1 and 2.
[0182] The x-axis represents an arbitrary direction in the plane of the optically absorptive anisotropic film, the y-axis represents a direction perpendicular to the x-axis in the film plane, and the z-axis represents the thickness direction of the optically absorptive anisotropic film. Ax represents the absorbance at the maximum absorption wavelength of the optically absorptive anisotropic film, and the absorbance of linearly polarized light vibrating in the x-axis direction. Ax (z=50) represents the absorbance at the maximum absorption wavelength when the optically absorptive anisotropic film is rotated 50° around the y-axis as the rotation axis, and the absorbance of linearly polarized light vibrating in the x-axis direction.
[0183] When measuring the absorbance, the measurement sample (1) was set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation, "UV-2450") and Ax was measured after correcting the absorbance at a wavelength of 800 nm to zero. For Ax (z = 50), the measurement sample (1) was set and tilted in the same manner, and Ax (z = 50) was measured after correcting the absorbance at a wavelength of 800 nm to zero.
[0184] [Haze measurement] (Initial haze measurement) The surface of the optical film on the first base layer side was attached to a glass of 4 cm × 4 cm × 0.7 mm thickness via a 25 μm thick pressure-sensitive adhesive (manufactured by Lintec Corporation) to obtain a measurement sample (2). For the measurement sample (2), light was incident on the glass surface using a haze meter HZ-1 (manufactured by Suga Test Instruments), and the haze was measured according to JIS K 7105, and this was defined as the initial haze. The results are shown in Tables 1 and 2.
[0185] (Haze measurement after durability test) The measurement sample (2) was heated at 100°C (dry condition) for 1 minute, and then cooled to room temperature (25°C) for 3 cycles. After this cycle was repeated, the haze was measured according to the procedure described in the measurement of the initial haze, and this was defined as the haze after the durability test. The results are shown in Tables 1 and 2.
[0186] [Clarity rating] The clarity was evaluated using the measurement sample (2) before and after the durability test used in the haze measurement. Specifically, the front glass was removed from a Samsung Galaxy S5 to remove the display device. The removed display device and the glass side of the measurement sample (2) after the durability test were placed on the display device with water between them. After that, the display device was turned on and the brightness was set to maximum, and all settings that change the screen display color, such as the blue light cut function and color balance change, were turned off, and the clarity when displaying white was evaluated with a white screen displayed (with the HTML color code #FFFFFF displayed). A: No deterioration in clarity was observed before and after the durability test. B: A slight decrease in clarity was observed before and after the durability test. C: A decrease in clarity was observed before and after the durability test.
[0187] [Table 1]
[0188] [Table 2] [Explanation of symbols]
[0189] 10 optical film, 11 light absorption anisotropic film, 12 first base layer (base layer), 20 elliptically polarizing plate, 21 polarizing element, 22 first retardation element, 23 second retardation element, 30 optical laminate.
Claims
1. A light absorbing anisotropic film formed from a composition containing one or more dichroic dyes and a polymerizable liquid crystal compound, the polymerizable liquid crystal compound includes a first liquid crystal compound and a second liquid crystal compound different from the first liquid crystal compound, each of the first liquid crystal compound and the second liquid crystal compound exhibits a smectic liquid crystal phase and contains two or more polymerizable groups in the molecule; The optically absorptive anisotropic film satisfies the relationships of the following formulas (1) and (2). 0.001≦Ax≦0.3 (1) Ax (z=50°) / Ax≧5 (2) [In formulas (1) and (2), Ax is the absorbance of the optically absorptive anisotropic film at the maximum absorption wavelength in the wavelength range of 380 nm to 780 nm, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Ax (z=50°) is the absorbance at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less when the optically absorptive anisotropic film is rotated 50° around the y axis as the rotation axis, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Here, the x-axis is any one direction within the plane of the optically absorptive anisotropic film, The y-axis is a direction perpendicular to the x-axis in the plane of the optically absorptive anisotropic film.
2. 2 . The optically absorptive anisotropic film according to claim 1 , wherein a total content of the first liquid crystal compound and the second liquid crystal compound is 99% by mass or more with respect to a total amount of the polymerizable liquid crystal compound.
3. The optically absorptive anisotropic film according to claim 1 , wherein each of the polymerizable groups is a (meth)acryloyl group.
4. The optically absorbing anisotropic film according to claim 1 , wherein the composition further comprises a non-liquid crystal compound having a reactive group.
5. 2. The optically absorptive anisotropic film according to claim 1, having a thickness of 0.1 μm or more and 3.0 μm or less.
6. 2. The optically absorptive anisotropic film according to claim 1, having a haze of 2.5% or less.
7. The first liquid crystal compound is a compound (a) represented by the following formula (a): The optically absorptive anisotropic film according to claim 1 , wherein the second liquid crystal compound is a compound (b) represented by the following formula (b): P1-F1-B1-G1-D1-G2-D2-G3-B2-F2-P2 (a) P3-F3-B3-G4-D3-G5-D4-G6-B4-F4-P4 (b) [In formula (a) and formula (b), D1 to D4 are each independently -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -C(=S)-O-, -O-C(=S)-, -O-C(=S)-O-, or -CO-NR 11 --, --NR 12 represents —CO— or a single bond; R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, B1 to B4 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, or -CO-NR 11 --, --NR 12 represents —CO— or a single bond; R 11 and R 12 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms, G1 to G6 each independently represent a divalent alicyclic hydrocarbon group having 3 to 16 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and a hydrogen atom contained in the alicyclic hydrocarbon group or the aromatic hydrocarbon group is not optionally substituted with a halogen atom, -R 13 , -OR 13 , cyano group, or nitro group; R 13 represents an alkyl group having 1 to 4 carbon atoms, and a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, F1 to F4 each independently represent an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group is -OR 14 or halogen atom, R 14 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom contained in the alkyl group may be substituted with a fluorine atom, and —CH 2 - may be replaced by -O- or -CO-; P1 to P4 represent a polymerizable group.
8. 8. The optically absorptive anisotropic film according to claim 7, wherein, in formulas (a) and (b), G1 and G4 are the same group, D1 and D3 are the same group, G2 and G5 are the same group, D2 and D4 are the same group, and G3 and G6 are the same group.
9. In the formulas (a) and (b), when the total number of carbon atoms contained in F1 and the total number of carbon atoms contained in F2 is C(a) and the total number of carbon atoms contained in F3 and the total number of carbon atoms contained in F4 is C(b), The optically absorptive anisotropic film according to claim 7 , wherein C(a) is greater than C(b).
10. 10. An optical film comprising the optically absorptive anisotropic film according to claim 1 and a substrate layer.
11. 11. An optical laminate comprising the light absorption anisotropic film according to any one of claims 1 to 9 or the optical film according to claim 10, and an elliptically polarizing plate.
Citation Information
Patent Citations
Vertically aligned liquid crystal cured film and laminate including the same
JP2020076920A