Circularly polarizing plate and organic el display device using the same
The circularly polarizing plate with controlled moisture content and specific film compositions addresses color change issues in organic EL displays by using a polarizing film and retardation film, ensuring stability in high-temperature conditions.
Patent Information
- Application Number
- JP2024148113
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-12
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-02-04
AI Technical Summary
Organic EL display devices face issues with color change due to water-induced hydrolysis of retardation films in high-temperature environments, caused by moisture in polarizing plates containing polyvinyl alcohol and dichroic dyes.
A circularly polarizing plate is designed with a polarizing film containing a dichroic dye and a transparent protective film, combined with a retardation film made from a cured polymerizable liquid crystal compound, maintaining an equilibrium water content of 1.5% or less to prevent color change.
The solution effectively prevents color change in high-temperature environments by controlling moisture content, ensuring stable performance of organic EL display devices.
Smart Images

Figure 2024159941000001 
Figure 2024159941000002 
Figure 2024159941000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a circular polarizing plate and an organic EL display device using the same. [Background technology]
[0002] In recent years, displays equipped with organic EL panels (organic EL display devices) have become widespread along with the spread of thin displays. Organic EL panels have a problem in that external light is reflected by the internal metal electrodes, making it impossible to obtain a clear black display. To address this problem, by providing a circular polarizing plate on the viewing surface, it is possible to suppress the prevention of external light reflection. In other words, the stacking order from the viewer is circular polarizing plate → organic EL display. Circular polarizing plates can generally be produced by stacking a polarizing plate and a retardation film. The polarizing plate is generally a polarizer made of PVA (polyvinyl alcohol) stretched and dyed with iodine, on which a transparent protective film is laminated, and the retardation film is a stretched film or a retardation film (λ / 4 plate) in which liquid crystal molecules are oriented. In this case, a λ / 4 plate that exhibits a property in which the longer the wavelength, the greater the birefringence (reverse wavelength dispersion characteristic) is preferably used. Summary of the Invention [Problem to be solved by the invention]
[0003] In organic EL display devices, there is a problem that the organic EL layer deteriorates due to oxygen and moisture depending on the usage environment and no longer emits light, so both sides of the organic EL panel may be protected by a substrate with low moisture permeability such as glass. In addition, the top surface of the panel may also be protected by a substrate with low moisture permeability from the water-resistant side. However, it was found that in such a configuration, depending on the type of retardation film, a problem occurs in that color changes occur in a high temperature environment. As a result of extensive investigation, it was found that a small amount of moisture contained in the protective film and polyvinyl alcohol that form the polarizing plate remains in the system, and the moisture causes hydrolysis of the retardation film, which causes color changes.
[0004] Therefore, an object of the present invention is to provide an excellent circular polarizing plate that exhibits little color change in a high-temperature environment, and an organic EL display device equipped with the circular polarizing plate. [Means for solving the problem]
[0005] The present invention relates to the following preferred embodiments [1] to
[12] . [1] A circular polarizing plate comprising a polarizing plate in which a polarizing film containing a dichroic dye and a transparent protective film having a thickness of 10 μm or more and 80 μm or less are laminated, and a retardation film which is a cured product of a composition containing a polymerizable liquid crystal compound B, The retardation film has a thickness of 5 μm or less, the polymerizable liquid crystal compound B is a compound having an ester bond in its molecular structure, The polarizing plate has an equilibrium moisture content of 1.5% by mass or less at a temperature of 23° C. and a relative humidity of 50%. [2] The circularly polarizing plate according to [1], wherein the dichroic dye is an azo dye. [3] The circularly polarizing plate according to [1] or [2], wherein the transparent protective film is made of a cyclic olefin resin. [4] The circularly polarizing plate according to any one of [1] to [3], wherein the polarizing film further contains a cured product of a polymerizable liquid crystal compound A having an acryloyloxy group or a methacryloyloxy group as a polymerizable group. [5] The circularly polarizing plate according to any one of [1] to [4], wherein the polarizing film exhibits a Bragg peak in X-ray diffraction measurement. [6] The circularly polarizing plate according to [4], wherein the cured product of the polymerizable liquid crystal compound A exhibits a smectic liquid crystal phase and is cured in a horizontally aligned state. [7] The circularly polarizing plate according to any one of [1] to [6], wherein the retardation film satisfies the following formula (1): 100 ≦ Re(550) ≦ 180 (1) [In the formula, Re(550) represents an in-plane retardation value at a wavelength of 550 nm.] [8] The circularly polarizing plate according to any one of [1] to [7], wherein the retardation film satisfies formula (2): Re(450) / Re(550)<1 (2) [In the formula, Re(450) and Re(550) represent in-plane retardation values at wavelengths of 450 nm and 550 nm, respectively.] [9] The circularly polarizing plate according to any one of [1] to [8], wherein the angle between the slow axis of the retardation film and the absorption axis of the polarizing film is substantially 45°.
[10] The circularly polarizing plate according to any one of [1] to [9], wherein the polymerizable liquid crystal compound B has at least one polymerizable group selected from an acryloyloxy group and a methacryloyloxy group.
[11] The circularly polarizing plate according to any one of [1] to
[10] , wherein the polymerizable liquid crystal compound B is a compound represented by the following formula (II): [ka] In formula (II), Ar represents a divalent aromatic group which may have a substituent. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. L 1 and L 2 each independently represents a divalent linking group having an ester structure. T 1 and T 2 each independently represents a single bond or a divalent linking group. h and i each independently represent an integer of 0 to 3, and satisfy the relationship 1≦h+i. In this case, when 2≦h+i, T 1 and T 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms, in which a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and -CH2- contained in the alkanediyl group may be substituted with -O-, -S- or -COO-, and when there are a plurality of -O-, -S- or -COO-, they are not adjacent to each other. P 1 and P 2each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
[12] The circularly polarizing plate according to any one of [1] to
[11] , wherein the polarizing plate has a transparent protective film laminated only on one side of the polarizing film.
[13] An organic electroluminescence display device comprising the circular polarizing plate according to any one of [1] to
[12] . Effect of the Invention
[0006] The circularly polarizing plate of the present invention can prevent color change even in a high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] A circular polarizing plate is composed of a polarizing plate and a retardation film. In the present invention, it is necessary to control the equilibrium moisture content of the polarizing plate at a temperature of 23°C and a humidity of 50% to 1.5 mass% or less. The equilibrium moisture content is defined as the moisture content in a state where the moisture content in a material reaches equilibrium in air at a constant temperature and humidity. In the present invention, a polarizing plate (size: width 4 cm, length 10 cm) is kept in a clean room at a temperature of 23°C and a relative humidity of 50% for one day and its mass is measured, and then the polarizing plate is dried at 105°C for one hour and its mass is measured, and the value calculated by the following formula is regarded as the equilibrium moisture content: (Mass at 23°C and 50% relative humidity - Mass after drying for 1 hour at 105°C) ÷ (Mass at 23°C and 50% relative humidity) x 100
[0008] In the present invention, if the equilibrium moisture content of the polarizing plate is higher than 1.5% by mass, the color of the circularly polarizing plate is likely to change at high temperatures, which is undesirable. The equilibrium moisture content of the polarizing plate is preferably 1.0% by mass or less, more preferably 0.5% by mass or less. The lower limit of the equilibrium moisture content of the polarizing plate may be 0. When the equilibrium moisture content of the polarizing plate is higher than 1.5% by mass, the equilibrium moisture content can be reduced by drying. Drying can be performed by heating or by leaving the polarizing plate in a dry environment, as appropriate.
[0009] The circular polarizing plate of the present invention includes a polarizing plate in which a polarizing film containing a dichroic dye and a transparent protective film having a thickness of 10 μm or more and 80 μm or less are laminated, and a retardation film which is a cured product of a composition containing a polymerizable liquid crystal compound B.
[0010] <Polarizing film> The polarizing film is a film having a function of light absorption anisotropy. The polarizing film may be a stretched film having a dichroic dye adsorbed thereon, or may be a cured product of a composition containing a horizontally aligned polymerizable liquid crystal compound and a horizontally aligned dichroic dye. From the viewpoint of the equilibrium water content, the polarizing film is more preferably a polarizing film made of a polymer of a polymerizable liquid crystal compound.
[0011] A film including, as a polarizing film, a stretched film having a dichroic dye adsorbed thereon is usually produced through a process of uniaxially stretching a polyvinyl alcohol-based resin film, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, a process of treating the polyvinyl alcohol-based resin film having the dichroic dye adsorbed thereon with an aqueous boric acid solution, and a process of washing with water after the treatment with the aqueous boric acid solution.
[0012] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. As polyvinyl acetate resins, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith are used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.
[0013] The degree of saponification of the polyvinyl alcohol resin is usually about 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can also be used. The degree of polymerization of the polyvinyl alcohol resin is usually about 1,000 to 10,000, preferably in the range of 1,500 to 5,000.
[0014] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizing film. The method for forming the polyvinyl alcohol-based resin is not particularly limited, and the film can be formed by a known method. The thickness of the polyvinyl alcohol-based raw film can be, for example, about 10 to 150 μm.
[0015] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. It is also possible to perform the uniaxial stretching at these multiple stages. In the uniaxial stretching, the film may be uniaxially stretched between rolls having different peripheral speeds, or may be uniaxially stretched using a heated roll. The uniaxial stretching may be dry stretching in which the film is stretched in the air, or wet stretching in which the polyvinyl alcohol-based resin film is stretched in a swollen state using a solvent. The stretching ratio is usually about 3 to 8 times.
[0016] Dyeing of a polyvinyl alcohol-based resin film with a dichroic dye is carried out, for example, by a method of immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye.
[0017] Specifically, iodine or a dichroic organic dye is used as the dichroic pigment. Examples of the dichroic organic dye include a dichroic direct dye made of a disazo compound such as CIDIRECT RED 39, and a dichroic direct dye made of a compound such as trisazo or tetrakisazo. It is preferable that the polyvinyl alcohol resin film is immersed in water before the dyeing process.
[0018] When iodine is used as the dichroic dye, a method is usually employed in which a polyvinyl alcohol resin film is immersed in an aqueous solution containing iodine and potassium iodide to dye it. The content of iodine in this aqueous solution is usually about 0.01 to 1 part by mass per 100 parts by mass of water. The content of potassium iodide is usually about 0.5 to 20 parts by mass per 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is usually about 20 to 40°C. The immersion time in this aqueous solution (dyeing time) is usually about 20 to 1,800 seconds.
[0019] On the other hand, when a dichroic organic dye is used as the dichroic coloring matter, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing a water-soluble dichroic dye is usually employed. The content of the dichroic organic dye in this aqueous solution is usually 1×10 -4 ~10 parts by mass, preferably 1 × 10 -3 ~1 part by mass, more preferably 1 × 10 -3 ~1×10 -2 The amount of the dye in the aqueous solution is expressed by parts by mass. This aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing assistant. The temperature of the aqueous dichroic dye solution used for dyeing is usually about 20 to 80° C. The immersion time in the aqueous solution (dyeing time) is usually about 10 to 1,800 seconds.
[0020] The boric acid treatment after dyeing with a dichroic dye can usually be carried out by immersing the dyed polyvinyl alcohol resin film in an aqueous boric acid solution. The content of boric acid in this aqueous boric acid solution is usually about 2 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. When iodine is used as the dichroic dye, this aqueous boric acid solution preferably contains potassium iodide, and in this case, the content of potassium iodide is usually about 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. The immersion time in the aqueous boric acid solution is usually about 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually 50°C or higher, preferably 50 to 85°C, and more preferably 60 to 80°C.
[0021] The polyvinyl alcohol-based resin film after the boric acid treatment is usually washed with water. The washing can be performed, for example, by immersing the polyvinyl alcohol-based resin film treated with boric acid in water. The temperature of the water used in the washing is usually about 5 to 40°C. The immersion time is usually about 1 to 120 seconds.
[0022] After washing with water, the film is dried to obtain a polarizing film. The drying can be performed using, for example, a hot air dryer or a far-infrared heater. The temperature of the drying is usually about 30 to 100°C, and preferably 50 to 80°C. The time of the drying is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content of the polarizer is reduced to a practical level by the drying. The moisture content is usually about 5 to 20% by mass, and preferably 8 to 15% by mass. If the moisture content is less than 5% by mass, the flexibility of the polarizing film is lost, and the polarizing film may be damaged or broken after drying. If the moisture content exceeds 20% by mass, the thermal stability of the polarizing film may be deteriorated.
[0023] The polyvinyl alcohol resin film is then uniaxially stretched, dyed with a dichroic dye, treated with boric acid, washed with water and dried to obtain a polarizing film having a thickness preferably of 5 to 40 μm.
[0024] In the case where the polarizing film is a cured product of a composition containing a horizontally aligned polymerizable liquid crystal compound and a horizontally aligned dichroic dye (hereinafter, sometimes referred to as a polymerizable liquid crystal composition (A)), the polymerizable liquid crystal compound may be a thermotropic liquid crystal or a lyotropic liquid crystal, but is preferably a thermotropic liquid crystal when mixed with a dichroic dye. In the case of a thermotropic liquid crystal, it may be a thermotropic liquid crystal compound exhibiting a nematic liquid crystal phase, or a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase. When the polymerizable liquid crystal compound is polymerized to exhibit a polarizing function as a cured film, the liquid crystal state exhibited by the polymerizable liquid crystal compound is preferably a smectic phase. Specific examples of such compounds will be described later.
[0025] The polymerizable liquid crystal composition (A) is a liquid crystal compound having at least one polymerizable group, and preferably contains a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity (hereinafter, also referred to as "polymerizable liquid crystal compound (A)"). By using a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, a polarizing film having a high degree of alignment order can be formed. The liquid crystal state exhibited by the polymerizable liquid crystal compound (A) is preferably a smectic phase (smectic liquid crystal state), and more preferably a high-order smectic phase (high-order smectic liquid crystal state) from the viewpoint of realizing a higher degree of orientation order. Here, the high-order smectic phase means a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, and a smectic L phase, and among these, the smectic B phase, the smectic F phase, and the smectic I phase are more preferable. The liquid crystal property may be a thermotropic liquid crystal or a lyotropic liquid crystal, but a thermotropic liquid crystal is preferable in terms of the possibility of precise film thickness control. In addition, the polymerizable liquid crystal compound may be a monomer, but may also be an oligomer or a polymer in which a polymerizable group is polymerized.
[0026] The polymerizable liquid crystal compound (A) is a liquid crystal compound having at least one polymerizable group. Here, the polymerizable group refers to a group that can participate in a polymerization reaction by an active radical or an acid generated from a polymerization initiator. Examples of the polymerizable group that the polymerizable liquid crystal compound (A) has include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, a radical polymerizable group is preferable, an acryloyloxy group, a methacryloyloxy group, a vinyl group, and a vinyloxy group are more preferable, and an acryloyloxy group and a methacryloyloxy group are even more preferable.
[0027] The polymerizable liquid crystal compound (A) is not particularly limited as long as it is a liquid crystal compound having at least one polymerizable group, and a known polymerizable liquid crystal compound can be used, for example, a compound represented by the following formula (A1) (hereinafter also referred to as "polymerizable liquid crystal compound (A1)"). U 1 -V 1 -W 1 -(X 1 -Y 1 -) n -X 2 -W 2 -V 2 -U 2 (A1) [In formula (A1), X 1 and X 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1 and X 2 At least one of these is a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent. Y 1 is a single bond or a divalent linking group. n is 1 to 3. If n is 2 or more, multiple X 1 may be the same or different. X 2 is multiple X 1 When n is 2 or more, a plurality of Y 1 may be the same as or different from each other. From the viewpoint of liquid crystallinity, n is preferably 2 or more. U 1 represents a hydrogen atom or a (meth)acryloyloxy group. U 2represents a (meth)acryloyloxy group. W 1 and W 2 are each independently a single bond or a divalent linking group. V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.]
[0028] In the polymerizable liquid crystal compound (A1), X 1 and X 2 are each independently preferably an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group; X 1 and X 2 At least one of the groups is a 1,4-phenylene group which may have a substituent, or a cyclohexane-1,4-diyl group which may have a substituent, and is preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent, or the cyclohexane-1,4-diyl group which may have a substituent, include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.
[0029] The polymerizable liquid crystal compound (A1) is represented by the formula (A1-1): -(X 1 -Y 1 -) n -X 2 - (A1-1) [In the formula, X 1 , Y 1 , X 2 and n have the same meanings as above. It is preferable that the portion represented by the following formula (hereinafter referred to as partial structure (A1-1)) has an asymmetric structure, since this facilitates the development of smectic liquid crystal properties. The polymerizable liquid crystal compound (A1) in which the partial structure (A1-1) is an asymmetric structure is, for example, a compound in which n is 1 and one X 1 and X 2 and Y are different from each other. 1 A compound in which two Xs are the same structure. 1 are identical in structure to each other, and one X 2 These two X 1 A polymerizable liquid crystal compound (A1) having a structure different from that of the two X 1 W of 1 X binds to 1 But the other X 1 and X 2 The structure is different from that of the other X 1 and X 2 Also included are polymerizable liquid crystal compounds (A1) having the same structure as each other. 1 are the same structure as each other, and three X 1 and 1 X 2 The polymerizable liquid crystal compound (A1) includes any one of the following three structures different from all of the other three structures.
[0030] Y 1 are -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or -CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is more preferably -CH2CH2-, -COO- or a single bond, 1 If present, X 2 Y that binds to 1 is more preferably -CH2CH2- or -CH2O-. 1 and X 2 When all of Y are the same structure, two or more Y1 It is preferable that there is a plurality of Y 1 When the compound has a structure of asymmetric structure, the compound tends to exhibit smectic liquid crystallinity.
[0031] U 2 is a (meth)acryloyloxy group. 1 is a hydrogen atom or a (meth)acryloyloxy group, and is preferably a (meth)acryloyloxy group. From the viewpoint of improving the adhesion between layers of the polarizing film and heat resistance, U 1 and U 2 are preferably both (meth)acryloyloxy groups. The (meth)acryloyloxy group may be in a polymerized state or an unpolymerized state, but is preferably in an unpolymerized state.
[0032] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.
[0033] Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted linear alkanediyl group.
[0034] W 1 and W 2 are each independently preferably a single bond, -O-, -S-, -COO- or -OCOO-, more preferably a single bond or -O-.
[0035] Specifically, the polymerizable liquid crystal compound (A) is preferably a polymerizable liquid crystal compound having a structure represented by formulae (Aa) to (Ai) and exhibiting smectic liquid crystallinity. From the viewpoint of easily exhibiting high-order smectic liquid crystallinity, it is more preferable that the compound has a structure represented by formula (Aa), formula (Ab) or formula (Ac). In formulae (Aa) to (Ai), * represents a bond (single bond).
[0036] [ka]
[0037] Specific examples of the polymerizable liquid crystal compound (A1) include compounds represented by formulae (A-1) to (A-25). When the polymerizable liquid crystal compound (A1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.
[0038] [ka]
[0039] [ka]
[0040] [ka]
[0041] [ka]
[0042] [ka]
[0043] Among these, at least one selected from the group consisting of compounds represented by formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17) is preferred. As the polymerizable liquid crystal compound (A1), one type may be used alone, or two or more types may be used in combination.
[0044] The polymerizable liquid crystal compound (A1) can be produced by a known method, for example, as described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), or Japanese Patent No. 4,719,156.
[0045] The polymerizable liquid crystal composition (A) may contain polymerizable liquid crystal compounds other than the polymerizable liquid crystal compound (A) as long as the effects of the present invention are not impaired. From the viewpoint of obtaining a polarizing film having a high degree of orientation order, the ratio of the polymerizable liquid crystal compound (A) to the total mass of all polymerizable liquid crystal compounds contained in the polymerizable liquid crystal composition (A) is preferably 51 mass% or more, more preferably 70 mass% or more, and even more preferably 90 mass% or more.
[0046] In addition, when the polymerizable liquid crystal composition (A) contains two or more polymerizable liquid crystal compounds (A), at least one of them may be the polymerizable liquid crystal compound (A1), or all of them may be the polymerizable liquid crystal compound (A1). By combining a plurality of polymerizable liquid crystal compounds, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature.
[0047] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition (A) is preferably 40 to 99.9% by mass, more preferably 60 to 99% by mass, and further preferably 70 to 99% by mass, based on the solid content of the polymerizable liquid crystal composition. When the content of the polymerizable liquid crystal compound is within the above range, the alignment of the polymerizable liquid crystal compound tends to be high. In this specification, the solid content refers to the total amount of components excluding the solvent from the polymerizable liquid crystal composition.
[0048] The polymerizable liquid crystal composition (A) contains a dichroic dye. Here, the dichroic dye means a dye having different properties between the absorbance in the long axis direction of the molecule and the absorbance in the short axis direction. The dichroic dye is a dye that exhibits dichroism by being oriented together with a liquid crystal compound, and the dichroic dye itself may have polymerizability or liquid crystal properties. The dichroic dye that can be used in the present invention is not particularly limited as long as it has the above-mentioned properties, and may be a dye or a pigment. In addition, two or more types of dyes or pigments may be used in combination, or a dye and a pigment may be used in combination.
[0049] Dichroic dyes have a maximum absorption wavelength (λ MAX ) is preferable. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes.
[0050] Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes. Bisazo dyes and trisazo dyes are preferred, and examples thereof include a compound represented by formula (I) (hereinafter also referred to as "compound (I)"). K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K. 3 each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K 2may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.
[0051] Examples of monovalent heterocyclic groups include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of divalent heterocyclic groups include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.
[0052] K 1 and K. 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 Examples of the substituent that the p-phenylene group, naphthalene-1,4-diyl group, and divalent heterocyclic group in the formula (I) may optionally have include an alkyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, and a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (a substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2).
[0053] Among the compounds (I), compounds represented by any one of the following formulas (I-1) to (I-6) are preferred. [ka] [In the formulas (I-1) to (I-8), B 1 ~B 30each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]
[0054] The anthraquinone dye is preferably a compound represented by formula (I-9). [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0055] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-8), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x, -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0056] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms. In formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.
[0057] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 represent, independently of each other, a group represented by any one of formulae (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 each independently represents a group represented by any one of formulas (I-13a) to (1-13h). [ka] n6 represents an integer from 1 to 3.
[0058] The content of the dichroic dye in the polymerizable liquid crystal composition (A) can be appropriately determined depending on the type of the dichroic dye used, and is preferably 0.1 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and even more preferably 0.1 to 12 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the dichroic dye is within the above range, the orientation of the polymerizable liquid crystal compound is unlikely to be disturbed, and a polarizing film having a high degree of orientation order can be obtained.
[0059] The polymerizable liquid crystal composition (A) may further contain a polymerization initiator. The polymerization initiator is a compound capable of initiating a polymerization reaction of the polymerizable liquid crystal compound, and a photopolymerization initiator is preferred in that the polymerization reaction can be initiated under lower temperature conditions. Specifically, photopolymerization initiators capable of generating active radicals or acids under the action of light can be mentioned, and among them, photopolymerization initiators that generate radicals under the action of light are preferred. The polymerization initiators can be used alone or in combination of two or more kinds.
[0060] Examples of the polymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, and a sulfonium salt.
[0061] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0062] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0063] Examples of the alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0064] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0065] The triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.
[0066] As the polymerization initiator, commercially available ones can be used. Examples of commercially available polymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", "Irgacure (registered trademark) 369" (Ciba Japan Co., Ltd.); "Seikuol (registered trademark) BZ", "Seikuol (registered trademark) Z", "Seikuol (registered trademark) 100", "Seikuol (registered trademark) 200", "Seikuol (registered trademark) 1 ... Examples of such compounds include "Kayacure (registered trademark) BEE" (Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.); "Kayacure (registered trademark) UVI-6992" (Dow Chemicals); "ADEKA Optomer SP-152", "ADEKA Optomer SP-170" (ADEKA Corporation); "TAZ-A", "TAZ-PP" (Nippon SiberHegner AG); and "TAZ-104" (Sanwa Chemical Co., Ltd.).
[0067] When the polymerizable liquid crystal composition (A) contains a polymerization initiator, the content thereof may be appropriately determined depending on the type and amount of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition (A), and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment.
[0068] When the polymerizable liquid crystal composition (A) contains a photopolymerization initiator, it may further contain a photosensitizer. The use of a photosensitizer can further promote the polymerization reaction of the polymerizable liquid crystal compound. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and an alkoxy group-containing anthracene (e.g., dibutoxyanthracene, etc.); phenothiazine, rubrene, etc. The photosensitizer can be used alone or in combination of two or more kinds.
[0069] The content of the photosensitizer in the polymerizable liquid crystal composition (A) may be appropriately determined depending on the type and amount of the photopolymerization initiator and the polymerizable liquid crystal compound, and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0070] The polymerizable liquid crystal composition (A) may further contain a leveling agent. The leveling agent has the function of adjusting the fluidity of the polymerizable liquid crystal composition (A) and making the coating film obtained by applying the polymerizable liquid crystal composition (A) flatter, and specifically includes a surfactant. As the leveling agent, at least one selected from the group consisting of leveling agents mainly composed of a polyacrylate compound and leveling agents mainly composed of a fluorine atom-containing compound is preferable. The leveling agents can be used alone or in combination of two or more kinds.
[0071] Examples of leveling agents based on polyacrylate compounds include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" (BYK Chemie).
[0072] Examples of leveling agents containing a fluorine atom-containing compound as a main component include "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" (DIC Corporation); "Surflon (registered trademark) S-381" and "S Examples of such products include "S-382", "S-383", "S-393", "SC-101", "SC-105", "KH-40" and "SA-100" (AGC Seimi Chemical Co., Ltd.); "E1830", "E5844" (Daikin Fine Chemical Research Institute, Ltd.); "F-TOP EF301", "F-TOP EF303", "F-TOP EF351" and "F-TOP EF352" (Mitsubishi Materials Electronic Chemicals Co., Ltd.).
[0073] The content of the leveling agent in the polymerizable liquid crystal composition (A) is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound is easily horizontally aligned, and unevenness is unlikely to occur, so that a smoother polarizing film tends to be obtained.
[0074] The polymerizable liquid crystal composition (A) may further contain additives other than the polymerization initiator, the photosensitizer, and the leveling agent. Examples of the additives include a release agent, a stabilizer, a colorant such as a bluing agent, a flame retardant, and a lubricant. When the polymerizable liquid crystal composition (A) contains other additives, the content of the other additives is preferably more than 0% and not more than 20% by mass, more preferably more than 0% and not more than 10% by mass, based on the solid content of the polymerizable liquid crystal composition (A).
[0075] The polymerizable liquid crystal composition (A) may further contain a solvent. Generally, a compound exhibiting smectic liquid crystallinity has a high viscosity, so that adding a solvent to the polymerizable liquid crystal composition makes it easy to apply the composition, and as a result, it is often easy to form a polarizing film. The solvent can be appropriately selected according to the solubility of the polymerizable liquid crystal compound and the dichroic dye, and specifically, for example, water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, and other alcohol solvents, ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, ethyl lactate, and other ester solvents, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, methyl isobutyl ketone, and other ketone solvents, pentane, hexane, heptane, and other aliphatic hydrocarbon solvents, toluene, xylene, and other aromatic hydrocarbon solvents, acetonitrile, and other nitrile solvents, tetrahydrofuran, dimethoxyethane, and other ether solvents, and chloroform, chlorobenzene, and other chlorinated hydrocarbon solvents, and the like can be mentioned. These solvents can be used alone or in combination of two or more. The content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and further preferably 180 to 600 parts by mass, relative to 100 parts by mass of the solid components constituting the polymerizable liquid crystal composition.
[0076] The polymerizable liquid crystal composition (A) can be produced by a conventionally known method for preparing a polymerizable liquid crystal composition, and can usually be prepared by mixing and stirring a polymerizable liquid crystal compound and a dichroic dye, as well as the above-mentioned additives and solvent, etc., as necessary.
[0077] When the polymerizable liquid crystal composition (A) contains a polymerizable liquid crystal compound that shows a smectic liquid crystal phase and hardens in a horizontally aligned state, it has an excellent effect of suppressing photodegradation of the dichroic dye, and a polarizing film in which the polarization performance is unlikely to decrease over time can be obtained from the polymerizable liquid crystal composition (A). In particular, when a polarizing film is made from the polymerizable liquid crystal composition (A) containing a polymerizable liquid crystal compound that shows a smectic liquid crystal phase and hardens in a horizontally aligned state, a polarizing film with a high degree of orientation order can be obtained.
[0078] A polarizing film having a high degree of orientation order shows a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase in X-ray diffraction measurement. The Bragg peak means a peak derived from a planar periodic structure of molecular orientation. Therefore, in a polarizing film formed from the polymerizable liquid crystal composition of the present invention, it is preferable that the polymerizable liquid crystal compound or its polymer is oriented so that the polarizing film shows a Bragg peak in X-ray diffraction measurement, and more preferably, the polymerizable liquid crystal compound is oriented in a "horizontal orientation" in which the molecules of the polymerizable liquid crystal compound are oriented in the direction in which light is absorbed. In the present invention, a polarizing film having a planar periodicity interval of the molecular orientation of 3.0 to 6.0 Å is preferable. A high degree of orientation order that shows a Bragg peak can be realized by controlling the type of polymerizable liquid crystal compound used, the type and amount of dichroic dye, etc.
[0079] The polarizing film in the present invention can be produced, for example, by forming a coating film of the polymerizable liquid crystal composition (A); removing the solvent from the coating; raising the temperature to a temperature at which the polymerizable liquid crystal compound (A) undergoes a phase transition to a liquid phase or higher, and then lowering the temperature to cause the polymerizable liquid crystal compound to undergo a phase transition to a smectic phase (smectic liquid crystal state); and The polymerizable liquid crystal compound is polymerized while maintaining the smectic phase (smectic liquid crystal state). The composition can be produced by a method comprising the steps of:
[0080] The coating film of the polymerizable liquid crystal composition (A) can be formed, for example, by applying the polymerizable liquid crystal composition (A), particularly the polymerizable liquid crystal composition (A) whose viscosity has been adjusted by adding a solvent (hereinafter, also referred to as "polarizing film-forming composition"), onto a substrate or an alignment film described later, etc. Alternatively, the polarizing film-forming composition may be directly applied onto a retardation film or other layers constituting the polarizing plate of the present invention.
[0081] Examples of a method for applying the composition for forming a polarizing film to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0082] Next, the solvent is removed by drying or the like under conditions in which the polymerizable liquid crystal compound (A) contained in the coating film obtained from the composition for forming a polarizing film does not polymerize, thereby forming a dried coating film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0083] Furthermore, in order to cause the polymerizable liquid crystal compound (A) to undergo a phase transition to a liquid phase, the temperature is raised to a temperature at which the polymerizable liquid crystal compound undergoes a phase transition to a liquid phase or higher, and then the temperature is lowered to cause the polymerizable liquid crystal compound to undergo a phase transition to a smectic phase (smectic liquid crystal state). Such a phase transition may be performed after removal of the solvent in the coating film, or may be performed simultaneously with removal of the solvent.
[0084] By polymerizing the polymerizable liquid crystal compound (A) while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound (A), a polarizing film is formed as a cured layer of the polymerizable liquid crystal composition (A). The polymerization method is preferably a photopolymerization method. In the photopolymerization, the light to be irradiated to the dried coating film is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of the polymerizable liquid crystal compound (A) (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound (A)) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams. Among them, ultraviolet light is preferred in that the progress of the polymerization reaction is easily controlled and that photopolymerization devices widely used in this field can be used. It is preferable to select the types of the polymerizable liquid crystal compound and the photopolymerization initiator contained in the polymerizable liquid crystal composition so that they can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can also be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. By adopting such a cooling means, the polymerization of the polymerizable liquid crystal compound can be carried out at a lower temperature, so that a polarizing film can be appropriately formed even if a substrate having a relatively low heat resistance is used. During photopolymerization, a patterned polarizing film can also be obtained by performing masking and development.
[0085] Examples of the light source of the active energy rays include a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, and a metal halide lamp.
[0086] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.
[0087] When the polarizing film is obtained by polymerizing the polymerizable liquid crystal compound (A) while maintaining the liquid crystal state of the smectic phase, it has an advantage that the polarizing performance is higher than that of a conventional host-guest type polarizing film (i.e., a polarizing film made of a liquid crystal state of a nematic phase) due to the action of the dichroic dye.Furthermore, it has an advantage that it has superior strength compared to those coated with only a dichroic dye or a lyotropic liquid crystal.
[0088] The thickness of the polarizing film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.1 to 10 μm, more preferably 0.3 to 4 μm, and further preferably 0.5 to 3 μm.
[0089] The polarizing film is preferably formed on an alignment film. The alignment film has an alignment regulating force that aligns the polymerizable liquid crystal compound (A) in a desired direction. The alignment film is preferably one that has solvent resistance that does not dissolve the polymerizable liquid crystal compound composition (A) when applied, and has heat resistance in a heat treatment for removing the solvent and orienting the polymerizable liquid crystal compound (A). Examples of such alignment films include alignment films containing an orienting polymer, photoalignment films, groove alignment films having a concave-convex pattern or a plurality of grooves on the surface, and stretched films stretched in the alignment direction. From the viewpoint of the accuracy of the alignment angle and the quality, a photoalignment film is preferable.
[0090] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.
[0091] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate and removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing (rubbing method). Examples of the solvent include the same solvents as those exemplified above as solvents that can be used when forming a polarizing film.
[0092] The concentration of the orienting polymer in the orienting polymer composition may be within a range in which the orienting polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.
[0093] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0094] The method for applying the orientable polymer composition to a substrate may be the same as those exemplified as the method for applying the composition for forming a polarizing film to a substrate.
[0095] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0096] In order to impart an alignment control force to the alignment film, a rubbing treatment can be carried out as necessary (rubbing method).
[0097] An example of a method for imparting an orientation control force by a rubbing method is to bring an oriented polymer film formed on the surface of a substrate by applying an oriented polymer composition to the substrate and annealing the composition into contact with a rotating rubbing roll wrapped with a rubbing cloth.
[0098] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film forming composition") to a substrate and irradiating the substrate with polarized light (preferably polarized UV). A photo-alignment film is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0099] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0100] Examples of the photoreactive group having a C=C bond include a vinyl group, a polyene group, a stilbene group, a stilbazolium group, a chalcone group, and a cinnamoyl group. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0101] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.
[0102] A photo-alignment-inducing layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the solvents exemplified above as the solvents that can be used when forming a polarizing film, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.
[0103] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the desired photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.
[0104] The method of applying the composition for forming a photo-alignment film to a substrate may be the same as the method of applying the alignment composition to a substrate. Examples of the method of removing the solvent from the applied composition for forming a photo-alignment film include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0105] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer to irradiate the polarized UV light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.
[0106] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0107] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film with multiple equally spaced linear grooves, the liquid crystal molecules are aligned in the direction along the grooves.
[0108] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form unevenness, followed by curing.
[0109] The thickness of the alignment film (alignment film containing an alignment polymer or photoalignment film) is usually in the range of 10 to 10,000 nm, preferably in the range of 10 to 1000 nm, more preferably 500 nm or less, further preferably 10 to 200 nm, and particularly preferably 50 to 150 nm.
[0110] The polarizing plate of the present invention is obtained by laminating a transparent protective film having a thickness of 10 μm or more and 80 μm or less on at least one side of the polarizing film via an adhesive composition. The adhesive composition is not particularly limited, and a known adhesive may be used. It is preferable that the polarizing plate of the present invention has a transparent protective film laminated on only one side of the polarizing film.
[0111] <Transparent protective film> The transparent protective film means a substrate having transparency capable of transmitting light, particularly visible light, and the transparency refers to a property in which the transmittance for light rays having a wavelength of 380 to 780 nm is 80% or more. Specific examples of the transparent protective film include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene-based polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide, and polyphenylene oxide. From the viewpoint of availability and transparency, polyethylene terephthalate, polymethacrylic acid esters, cellulose esters, cyclic olefin resins, and polycarbonates are preferred. Cellulose esters are esters in which a part or all of the hydroxyl groups contained in cellulose are esterified, and are easily available on the market. Cellulose ester substrates are also easily available on the market. Examples of commercially available cellulose ester substrates include "FUJITAC FILM" (Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (Konica Minolta Opto Co., Ltd.). Among these, from the viewpoint of equilibrium water content, cyclic olefin resins, polyethylene terephthalate and polycarbonate are preferred, and cyclic olefin resins are more preferred.
[0112] The properties required for the transparent protective film vary depending on the configuration of the polarizing plate, but generally, a film with as small a retardation as possible is preferred. Examples of films with as small a retardation as possible include cellulose ester films with no retardation, such as Zerotack (Konica Minolta Opto, Inc.) and Z-tack (Fujifilm Corporation). Unstretched cyclic olefin resin films are also preferred. The surface of the transparent protective film on which the polarizing film is not laminated may be subjected to hard coat treatment, antireflection treatment, antistatic treatment, etc.
[0113] If the transparent protective film is too thin, the strength decreases and the processability tends to be poor, so the thickness is usually 10 to 80 μm, preferably 20 to 60 μm, and more preferably 20 to 40 μm.
[0114] <Retardation film> In the present invention, the retardation film is represented by the following formula (1): 100 ≦ Re(550) ≦ 180 (1) (wherein Re(550) represents an in-plane retardation value at a wavelength of 550 nm) It is preferable that the following is satisfied. When the retardation film has an in-plane retardation value represented by the above formula (1), it functions as a so-called λ / 4 plate. The formula (1) is preferably 100 nm≦Re(550)≦180 nm, and more preferably 120 nm≦Re(550)≦160 nm. Note that Re(550) can be measured by the method described in the Examples.
[0115] Furthermore, the retardation film has the following formula (2): Re(450) / Re(550) < 1 (2) (In the formula, Re(450) and Re(550) represent in-plane retardation values at wavelengths of 450 nm and 550 nm, respectively.) It is preferable that the above formula (2) is satisfied. A retardation film satisfying the above formula (2) has a so-called reverse wavelength dispersion and exhibits excellent polarization performance. The value of Re(450) / Re(550) is preferably 0.93 or less, more preferably 0.88 or less, even more preferably 0.86 or less, preferably 0.80 or more, more preferably 0.82 or more.
[0116] The retardation film is generally obtained by polymerizing a polymerizable liquid crystal compound in an aligned state. The polymerizable liquid crystal compound (hereinafter also referred to as "polymerizable liquid crystal compound B") forming the retardation film means a liquid crystal compound having a polymerizable group, particularly a photopolymerizable group. The photopolymerizable group means a group that can participate in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator. Examples of the photopolymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, an acryloyloxy group and a methacryloyloxy group are more preferred, and an acryloyloxy group is even more preferred. The liquid crystal property may be a thermotropic liquid crystal or a lyotropic liquid crystal, and the phase order structure may be a nematic liquid crystal or a smectic liquid crystal. As the polymerizable liquid crystal compound B, one type may be used alone, or two or more types may be used in combination.
[0117] As the polymerizable liquid crystal compound B, from the viewpoints of easiness of film formation and imparting the property represented by the above formula (Y), a compound satisfying all of the following (a) to (d) can be mentioned.
[0118] (A) A compound having thermotropic liquid crystallinity; (a) The polymerizable liquid crystal compound has π electrons in the long axis direction (a). (c) It has π electrons in a direction intersecting with the long axis direction (a) [intersecting direction (b)]. (D) The total number of π electrons present in the long axis direction (a) is N(πa), and the total number of molecular weights present in the long axis direction is N(Aa), where N(πa) is the total number of π electrons present in the long axis direction, and N(Aa) is the total number of molecular weights present in the long axis direction. The π electron density in the long axis direction (a) of a polymerizable liquid crystal compound is defined by the following formula (i): D(πa)=N(πa) / N(Aa) (i) The total number of π electrons present in the cross direction (b) is N(πb), and the total number of molecular weights present in the cross direction (b) is N(Ab), where N(πb) is the total number of π electrons present in the cross direction (b), and the π electron density in the cross direction (b) of the polymerizable liquid crystal compound is defined by the following formula (ii): D(πb)=N(πb) / N(Ab) (ii) But, 0≦[D(πa) / D(πb)]≦1 (i.e., the π electron density in the cross direction (b) is greater than the π electron density in the long axis direction (a).) The polymerizable liquid crystal compound B satisfying all of the above (A) to (D) can form a nematic phase by applying it onto an alignment film formed by rubbing treatment and heating it to a temperature equal to or higher than the phase transition temperature. In the nematic phase formed by the alignment of the polymerizable liquid crystal compound B, the long axis directions of the polymerizable liquid crystal compounds are usually aligned so as to be parallel to each other, and the long axis direction becomes the alignment direction of the nematic phase.
[0119] The polymerizable liquid crystal compound B having the above characteristics generally exhibits reverse wavelength dispersion. Specific examples of the compound satisfying the above characteristics (a) to (d) include compounds represented by the following formula (II): [ka] The compounds represented by the formula (II) can be used alone or in combination of two or more kinds.
[0120] In formula (II), Ar represents a divalent aromatic group which may have a substituent. The aromatic group here refers to a group having a planar cyclic structure, and the number of π electrons of the cyclic structure is [4n+2] according to the Huckel rule. Here, n represents an integer. When a ring structure is formed by including heteroatoms such as -N= or -S-, the non-covalent bond electron pairs on these heteroatoms also satisfy the Huckel rule and have aromaticity. The divalent aromatic group preferably includes at least one of a nitrogen atom, an oxygen atom, and a sulfur atom.
[0121] G 1 and G 2each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom.
[0122] L 1 and L 2 each independently represents a divalent linking group having an ester structure. T 1 and T 2 each independently represents a single bond or a divalent linking group.
[0123] h and i each independently represent an integer of 0 to 3, and satisfy the relationship of 1≦h+i. In this case, when 2≦h+i, T 1 and T 2 , G 1 and G 2 may be the same as or different from each other.
[0124] E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms, in which a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and -CH2- contained in the alkanediyl group may be substituted with -O-, -S-, -Si-, or -COO-. 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
[0125] G 1 and G 2are each independently preferably a 1,4-phenylenediyl group which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, more preferably a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group. 1 and G 2 At least one of L is preferably a divalent alicyclic hydrocarbon group. 1 or L 2 G binds to 1 and G 2 It is more preferable that at least one of the groups is a divalent alicyclic hydrocarbon group.
[0126] L 1 and L 2 are each independently preferably -R a1 COOR a2 -(R a1 and R a2 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, and more preferably -COOR a2-1 -(R a2-1 represents a single bond, -CH2-, or -CH2CH2-, and more preferably -COO- or -COOCH2CH2-.
[0127] T 1 and T 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -, -R a11 COOR a12 -, -R a13 OCOR a14 - or R a15 OC=OORa16 -, where R a9 ~R a16 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and T 2 are each independently preferably a single bond, -OR a10-1 -, -CH2-, -CH2CH2-, -COOR a12-1 - or O.C.O.R. a14-1 -, where R a10-1 , R a12-1 , R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. T 1 and T 2 are each independently more preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or OCOCH2CH2-.
[0128] From the viewpoint of expressing reverse wavelength dispersion, h and i are preferably in the range of 2≦h+i≦6, preferably h+i=4, and more preferably h=2 and i=2. When h=2 and i=2, a symmetric structure is obtained, which is even more preferable.
[0129] E 1 and E 2 are each independently preferably an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms.
[0130] P 1 or P 2 Examples of the polymerizable group represented by the formula (I) include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred.
[0131] It is preferable that Ar has at least one selected from an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, and an electron-withdrawing group. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring, and the like, and the benzene ring and the naphthalene ring are preferable. Examples of the aromatic heterocycle include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring. Among these, it is preferable that Ar has a thiazole ring, a benzothiazole ring, or a benzofuran ring, and it is more preferable that Ar has a benzothiazole group. In addition, when Ar contains a nitrogen atom, it is preferable that the nitrogen atom has π electrons.
[0132] In formula (II), the total number of π electrons contained in the divalent aromatic group represented by Ar is N π is preferably 8 or more, more preferably 10 or more, even more preferably 14 or more, and particularly preferably 16 or more. Also, it is preferably 30 or less, more preferably 26 or less, and even more preferably 24 or less.
[0133] Examples of the aromatic group represented by Ar include groups of the following formulae (Ar-1) to (Ar-23).
[0134] [ka]
[0135] In formulae (Ar-1) to (Ar-23), * represents a linking portion, Z 0 , Z 1 and Z 2each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.
[0136] Q 1 and Q 2 are each independently -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ -, -CO- or O-; R 2’ and R 3’ each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0137] J 1 and J. 2 each independently represents a carbon atom or a nitrogen atom.
[0138] Y 1 , Y 2 and Y 3 each independently represents an optionally substituted aromatic hydrocarbon group or an optionally substituted aromatic heterocyclic group.
[0139] W 1 and W 2 each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom; and m represents an integer of 0 to 6.
[0140] Y 1 , Y 2 and Y 3Examples of the aromatic hydrocarbon group in the formula (I) include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a biphenyl group, of which a phenyl group and a naphthyl group are preferred, and a phenyl group is more preferred. Examples of the aromatic heterocyclic group in the formula (I) include aromatic heterocyclic groups having 4 to 20 carbon atoms and containing at least one heteroatom, such as a nitrogen atom, an oxygen atom, or a sulfur atom, such as a furyl group, a pyrrolyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group, of which a furyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group are preferred.
[0141] Y 1 and Y 2 may each independently be an optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.
[0142] Z 0 , Z 1 and Z 2 are each preferably independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms; Z 0 is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group; Z 1 and Z 2 is more preferably a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group.
[0143] Q 1 and Q 2 -NH-, -S-, -NR 2’ -, -O- are preferred, R 2’ is preferably a hydrogen atom, and among these, -S-, -O-, and -NH- are particularly preferable.
[0144] Among the formulae (Ar-1) to (Ar-23), the formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.
[0145] In formulas (Ar-17) to (Ar-23), Y 1 is the nitrogen atom to which it is bonded and Z 0 and may form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those mentioned above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. This aromatic heterocyclic group may have a substituent. In addition, Y 1 is the nitrogen atom to which it is bonded and Z 0 In addition, it may be the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. For example, it may be a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc. The compound represented by the formula (II) can be produced, for example, according to the method described in JP-A-2010-31223.
[0146] The content of the polymerizable liquid crystal compound B in the polymerizable liquid crystal composition (B) constituting the retardation film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, and more preferably 90 to 98 parts by mass, based on 100 parts by mass of the solid content of the polymerizable liquid crystal composition (B). When the content is within the above range, the alignment of the retardation film tends to be high. Here, the solid content refers to the total amount of components excluding volatile components such as solvents from the polymerizable liquid crystal composition (B).
[0147] The polymerizable liquid crystal composition (B) may contain a polymerization initiator for initiating a polymerization reaction of the polymerizable liquid crystal compound B. Examples of the polymerization initiator include those exemplified above as polymerization initiators usable in the polymerizable liquid crystal composition (A). The polymerizable liquid crystal composition (B) may also contain, as necessary, a photosensitizer, a leveling agent, and additives exemplified as additives contained in the polymerizable liquid crystal composition (A). Examples of the photosensitizer and leveling agent include those exemplified above as additives usable in the polymerizable liquid crystal composition (A).
[0148] The retardation film can be obtained by applying a composition (hereinafter also referred to as a "composition for forming a retardation film") prepared by adding a solvent to a polymerizable liquid crystal composition (B) containing a polymerizable liquid crystal compound B and, if necessary, a polymerization initiator, an additive, etc., and mixing and stirring the composition on a substrate or an alignment film, removing the solvent by drying, and curing the polymerizable liquid crystal compound B in the resulting coating film by heating and / or active energy rays. Examples of the substrate and / or alignment film used for producing the retardation film include the same ones as those exemplified above as those usable for producing the above-mentioned polarizing film.
[0149] The solvent used in the composition for forming a retardation film, the method for applying the composition for forming a retardation film, the conditions for curing with active energy rays, and the like are all the same as those that can be used in the above-mentioned method for producing a polarizing film.
[0150] The thickness of the retardation film can be appropriately selected depending on the display device to which it is applied, but from the viewpoints of thinning and flexibility, it is preferably 0.1 to 10 μm, more preferably 1 to 5 μm, and even more preferably 1 to 3 μm.
[0151] <Circular polarizing plate> The circular polarizing plate of the present invention comprises the above-mentioned polarizing plate and a retardation film, and the above-mentioned polarizing plate is preferably formed by laminating a transparent protective film, an alignment film (particularly a photoalignment film), and a polarizing film in this order. In the circular polarizing plate of the present invention, it is preferable that the polarizing plate has a transparent protective film laminated on only one side of the polarizing film, and it is further preferable that the polarizing film and the retardation film are laminated. The circularly polarizing plate of the present invention may further include layers other than the polarizing plate and the retardation film (such as a protective layer and a pressure-sensitive adhesive layer). In the circular polarizing plate of the present invention, the above-mentioned polarizing film and the retardation film may be bonded to each other via an adhesive layer or a pressure-sensitive adhesive layer, or the retardation film may be formed directly on the polarizing film of the present invention by directly applying a composition for forming a retardation film to the above-mentioned polarizing film.
[0152] In the circular polarizing plate of the present invention, the angle between the slow axis of the retardation film and the absorption axis of the polarizing film is preferably substantially 45°. In the present invention, "substantially 45°" means 45°±5°.
[0153] The thickness of the circularly polarizing plate of the present invention is preferably from 10 to 300 μm, more preferably from 20 to 200 μm, and further preferably from 25 to 100 μm, from the viewpoints of flexibility and visibility of the display device.
[0154] <Display device> The present invention includes a display device comprising the circular polarizing plate of the present invention. The display device of the present invention can be obtained, for example, by bonding the polarizing film or polarizing plate of the present invention to the surface of a display device via an adhesive layer. The circular polarizing plate of the present invention exhibits a greater effect when the circular polarizing plate has a hydrophobic substrate on both sides. The hydrophobic substrate refers to a substrate having a moisture permeability of 10 g / m2·d (40°C·90% RH) (JISK 7129) or less. The type of hydrophobic substrate is not particularly limited, but examples thereof include glass. A display device is a device having a display mechanism, and includes a light-emitting element or a light-emitting device as a light source. Examples of display devices include liquid crystal display devices, organic electroluminescence (EL) display devices, inorganic electroluminescence (EL) display devices, touch panel display devices, electron emission display devices (field emission displays (FEDs, etc.), surface field emission displays (SEDs)), electronic paper (display devices using electronic ink or electrophoretic elements), plasma display devices, projection display devices (grating light valve (GLV) display devices, displays having digital micromirror devices (DMDs), etc.), and piezoelectric ceramic displays. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection liquid crystal display device. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images. In particular, the display device of the present invention is preferably an organic EL display device or a touch panel display device, and more preferably an organic EL display device. EXAMPLES
[0155] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, "%" and "parts" are "% by mass" and "parts by mass" unless otherwise specified.
[0156] [Example 1] <Preparation of polarizing plate> [Polarizing Plate: Manufacture of Polarizing Plate Containing Polarizing Film Formed from Stretched Film] A 30 μm thick polyvinyl alcohol film (average degree of polymerization: about 2400, saponification degree: 99.9 mol% or more) was uniaxially stretched about 5 times by dry stretching, and then, while maintaining the tension, was immersed in pure water at 40° C. for 40 seconds. After that, it was immersed in a dyeing solution with a mass ratio of iodine / potassium iodide / water of 0.044 / 5.7 / 100 at 28° C. for 30 seconds to perform a dyeing process. Next, the film was immersed in an aqueous boric acid solution with a mass ratio of potassium iodide / boric acid / water of 11.0 / 6.2 / 100 at 70° C. for 120 seconds. Subsequently, the film was washed with pure water at 8° C. for 15 seconds, and then dried at 60° C. for 50 seconds and then at 75° C. for 20 seconds while being held under a tension of 300 N, to obtain a polarizer having a thickness of 12 μm in which iodine was adsorbed and aligned in the polyvinyl alcohol film.
[0157] A water-based adhesive was poured between the obtained polarizer and a cycloolefin film (ZF14 manufactured by Zeon Corporation), and the two were laminated with a nip roll. The resulting laminate was dried at 60°C for 2 minutes while maintaining the tension at 430N / m, to obtain a polarizing plate I having a cycloolefin film as a transparent protective film on one side. The water-based adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318; manufactured by Kuraray Co., Ltd.) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650; manufactured by Sumika Chemtex Corporation, an aqueous solution with a solid content of 30%) to 100 parts of water.
[0158] <Equilibrium moisture content of polarizing plate at 23℃ 50%> A test piece of the prepared polarizing plate (size: width 4 cm, length 10 cm) was kept in a clean room at 23°C and 50% relative humidity for one day and its weight was measured, then the test piece was dried at 105°C for one hour and its weight was measured, and its equilibrium moisture content at a temperature of 23°C and a relative humidity of 50% was measured using a Mitsubishi Chemical Analytech CA-200. The results are shown in Table 1.
[0159] <Preparation of retardation film> [Preparation of composition for forming photoalignment film] 5 parts of the following photoalignment material (number average molecular weight 28000) and 95 parts of cyclopentanone (solvent) were mixed, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photoalignment film.
[0160] [ka]
[0161] [Preparation of polymerizable liquid crystal composition] Polymerizable liquid crystal compound B1 (86.0 parts) having the following structure, polymerizable liquid crystal compound A1 (14.0 parts), polyacrylate compound (leveling agent) (BYK-361N; manufactured by BYK-Chemie) (0.12 parts), and photopolymerization initiator 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) (3.0 parts) were mixed to obtain a polymerizable liquid crystal composition (B1) containing the polymerizable liquid crystal compound B1 and the polymerizable liquid crystal compound A1.
[0162] Polymerizable liquid crystal compound B1: [ka]
[0163] Polymerizable liquid crystal compound A1: [ka]
[0164] [Method of manufacturing phase difference film] A cycloolefin polymer film (COP; ZF-14; Zeon Corporation) was treated once using a corona treatment device (AGF-B10; Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The photoalignment film-forming composition was applied to the corona-treated surface with a bar coater, dried at 80°C for 1 minute, and then irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7 with polarizer unit; Ushio Inc.). 2 The thickness of the resulting alignment film was measured with an ellipsometer M-220 (manufactured by JASCO Corporation) and found to be 100 nm.
[0165] Next, the polymerizable liquid crystal composition B1 was applied onto the alignment film at a speed of 50 mm / sec by setting the wire of a bar coater to #30, and then dried for 1 minute at 120° C. Thereafter, ultraviolet light was irradiated from the side on which the polymerizable liquid crystal composition B1 was applied using a high-pressure mercury lamp (Unicur VB-15201BY-A; manufactured by Ushio Inc.) (under a nitrogen atmosphere, cumulative light amount at a wavelength of 313 nm: 500 mJ / cm 2 ) to form a laminate of the retardation film A and the cycloolefin polymer film. The thickness of the obtained retardation film A was measured with a laser microscope (LEXT; manufactured by Olympus Corporation) and was found to be 2.3 μm.
[0166] <Preparation of circular polarizing plate>
[0167] The polyvinyl alcohol side of the polarizing plate I prepared as described above and the retardation film A side of the laminate of retardation film A and cycloolefin polymer film were bonded together using an acrylic pressure-sensitive adhesive (colorless, transparent, non-oriented) so that the angle (θ) between the absorption axis of the polarizing plate I and the slow axis of the retardation film A was 45°, and then the cycloolefin polymer film of the retardation film was peeled off to produce a circular polarizing plate.
[0168] <Durability test> The obtained circular polarizing plate was attached to a 0.4 mm thick glass (manufactured by Corning) on both sides of the retardation film and the polarizing plate via an acrylic pressure-sensitive adhesive (colorless, transparent, non-oriented), and the retardation value of the retardation film was measured. After that, it was placed in a 90°C RH oven for 500 hours, and the retardation value of the retardation film was measured again to obtain the difference. The difference in the retardation values is shown in Table 1. The durability evaluation is also shown in Table 1 according to the following criteria. Durability evaluation ○: Difference is less than 1 nm. △: Difference is 1 nm or more and less than 10 nm. ×: Difference is 10 nm or more. Table 1 shows the materials constituting the polarizing plates and the main materials constituting the retardation films.
[0169] [Example 2] <Preparation of polarizing plate> [Polarizing plate: Production of a polarizing plate including a polarizing film formed from a composition including a polymerizable liquid crystal compound] (Production of composition for forming alignment layer) Two parts of the polymer described below and 98 parts of o-xylene were mixed, and the resulting mixture was stirred at 80° C. for one hour to obtain a composition for forming an alignment layer, which is a composition for forming a photoalignment film.
[0170] -2 parts of the polymer (number average molecular weight 28,000) having the photoreactive group shown below [ka]
[0171] (Production of composition for forming polarizing layer) The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming a polarizing layer.
[0172] 75 parts of a polymerizable liquid crystal compound represented by formula (1-6) [ka]
[0173] 25 parts of a polymerizable liquid crystal compound represented by formula (1-7) [ka]
[0174] 2.8 parts of the dichroic dye (1) shown below [ka]
[0175] 2.8 parts of the dichroic dye (2) shown below [ka]
[0176] 2.8 parts of the dichroic dye (3) shown below [ka]
[0177] 6 parts of the polymerization initiator shown below 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals)
[0178] 1.2 parts of the leveling agent shown below Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)
[0179] 250 parts of the following solvent Cyclopentanone
[0180] (Manufacture of polarizing plates) The surface of a triacetyl cellulose film (TAC; KC2UA; manufactured by Konica Minolta, Inc.) serving as a base material (transparent protective film) layer was subjected to a corona treatment (AGF-B10, manufactured by Kasuga Electric Co., Ltd.). The composition for forming an alignment layer was applied to the corona-treated film surface using a bar coater, and then dried for 1 minute in a drying oven set at 120°C to obtain a coating layer for the alignment layer. Polarized UV was irradiated onto the coating layer for the alignment layer at 50 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 An alignment layer was formed by irradiating the film with an integrated light amount (based on 313 nm). A composition for forming a polarizing layer was applied onto the obtained alignment layer using a bar coater, and then dried for 1 minute in a drying oven set at 110°C. Thereafter, ultraviolet light was irradiated using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, integrated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to obtain a polarizing plate in which the polymerizable liquid crystal compound and the dichroic dye were aligned. Except for using this polarizing plate, a circular polarizing plate was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0181] [Example 3] A polarizing plate and a circular polarizing plate were produced and evaluated in the same manner as in Example 2, except that a cycloolefin polymer film (COP; ZF-14; manufactured by Zeon Corporation) was used as the base material (transparent protective film) layer instead of the triacetyl cellulose film. The results are shown in Table 1.
[0182] [Example 4] A polarizing plate and a circular polarizing plate were prepared and evaluated in the same manner as in Example 2, except that the polymerizable liquid crystal compound B1 was replaced with the polymerizable compound B2 described in JP-A-2016-81035 for the retardation film. The results are shown in Table 1. Polymerizable compound B2 [ka]
[0183] [Example 5] A polarizing plate and a circularly polarizing plate were produced and evaluated in the same manner as in Example 2, except that the following polymerizable liquid crystal compound B3 was used in place of the polymerizable liquid crystal compound B1 for the retardation film. The results are shown in Table 1. Polymerizable compound B3 [ka]
[0184] [Comparative Example 1] A polarizing plate and a circular polarizing plate were produced and evaluated in the same manner as in Example 1, except that triacetyl cellulose films (TAC; KC2UA; manufactured by Konica Minolta, Inc.) were used as transparent protective films on both sides of the polarizer. The results are shown in Table 1.
[0185] [Comparative Example 2] A polarizing plate and a circular polarizing plate were produced and evaluated in the same manner as in Example 1, except that a triacetyl cellulose film (TAC; KC2UA; manufactured by Konica Minolta, Inc.) was used on one side as a protective film for the polarizing plate, and a cycloolefin polymer film (COP; ZF-14; manufactured by Zeon Corporation) was used on the other side, and a retardation layer was attached to the triacetyl cellulose film side of the polarizing plate. The results are shown in Table 1.
[0186] [Comparative Example 3] A polarizing plate and a circularly polarizing plate were produced and evaluated in the same manner as in Comparative Example 2, except that the same polymerizable liquid crystal compound as in Example 4 was used as the polymerizable liquid crystal compound of the retardation film. The results are shown in Table 1.
[0187] [Comparative Example 4] A polarizing plate and a circularly polarizing plate were produced and evaluated in the same manner as in Comparative Example 2, except that the same polymerizable liquid crystal compound as in Example 5 was used as the polymerizable liquid crystal compound of the retardation film.
[0188] [Reference example 1] A polarizing plate and a circular polarizing plate were produced and evaluated in the same manner as in Comparative Example 1, except that a cycloolefin polymer film (COP; ZD-12; manufactured by Zeon Corporation) was used as the retardation film. The results are shown in Table 1.
[0189] [Table 1]
[0190] As is clear from the results in Table 1 above, the equilibrium moisture content of the polarizing plate at 23°C and 50% (relative humidity) is 1.5% or less in Examples 1 to 5, and the durability in those cases is rated as O or △, whereas the durability in Comparative Examples 1 to 4, in which the equilibrium moisture content exceeds 1.5%, is rated as ×, and the difference in the results is clear. In Reference Example 1, even when the equilibrium moisture content of the polarizing plate exceeds 1.5%, the durability was good when the retardation film was made of a stretched film (retardation film not containing a polymerizable liquid crystal compound). It is considered that the retardation film is not affected by the moisture in the polarizing plate.
Claims
1. A circular polarizing plate comprising a polarizing plate in which a polarizing film containing a dichroic dye and a transparent protective film having a thickness of 10 μm or more and 80 μm or less are laminated, and a retardation film which is a cured product of a composition containing a polymerizable liquid crystal compound B, The retardation film has a thickness of 5 μm or less, the polymerizable liquid crystal compound B is a compound having an ester bond in a molecular structure, The polarizing plate has an equilibrium moisture content of 1.5% by mass or less at a temperature of 23° C. and a relative humidity of 50%.
2. 2. The circular polarizing plate according to claim 1, wherein the dichroic dye is an azo dye.
3. 3. The circularly polarizing plate according to claim 1, wherein the transparent protective film is made of a cyclic olefin resin.
4. 4. The circularly polarizing plate according to claim 1, wherein the polarizing film further comprises a cured product of a polymerizable liquid crystal compound A having an acryloyloxy group or a methacryloyloxy group as a polymerizable group.
5. 5. The circular polarizing plate according to claim 1, wherein the polarizing film exhibits a Bragg peak in X-ray diffraction measurement.
6. 5. The circularly polarizing plate according to claim 4, wherein the cured product of the polymerizable liquid crystal compound A is cured in a state of horizontal alignment exhibiting a smectic liquid crystal phase.
7. 7. The circularly polarizing plate according to claim 1, wherein the retardation film satisfies the following formula (1): 100≦Re(550)≦180 (1) [In the formula, Re(550) represents an in-plane retardation value at a wavelength of 550 nm.]
8. 8. The circularly polarizing plate according to claim 1, wherein the retardation film satisfies formula (2). Re(450) / Re(550)<1 (2) [In the formula, Re(450) and Re(550) represent in-plane retardation values at wavelengths of 450 nm and 550 nm, respectively.]
9. 9. The circular polarizing plate according to claim 1, wherein the angle between the slow axis of the retardation film and the absorption axis of the polarizing film is substantially 45°.
10. 10. The circular polarizing plate according to claim 1, wherein the polymerizable liquid crystal compound B has at least one polymerizable group selected from the group consisting of an acryloyloxy group and a methacryloyloxy group.
11. 11. The circularly polarizing plate according to claim 1, wherein the polymerizable liquid crystal compound B is a compound represented by the following formula (II): 【Chemistry 1】 In formula (II), Ar represents a divalent aromatic group which may have a substituent. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. L 1 and L 2 each independently represents a divalent linking group having an ester structure. T 1 and T 2 each independently represents a single bond or a divalent linking group. h and i each independently represent an integer of 0 to 3, and satisfy the relationship 1≦h+i. Here, when 2≦h+i, T 1 and T 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms, wherein a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and —CH 2 - may be replaced by -O-, -S- or -COO-, and when there are a plurality of -O-, -S- or -COO-, they are not adjacent to each other. P 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
12. 12. The circularly polarizing plate according to claim 1, wherein the polarizing plate has a transparent protective film laminated on only one side of the polarizing film.
13. An organic EL display device comprising the circular polarizer according to any one of claims 1 to 12.
Citation Information
Patent Citations
Laminated optical element and liquid crystal display device
JP2001337225A
Liquid crystal display
JP2005173567A
Liquid crystal display device
JP2010085696A
Circularly polarizing plate and display device
JP2014063143A
Transparent film, manufacturing method therefor, transparent conductive film, touch panel, Anti-reflection film, polarizing plate, and display device