Nonaqueous electrolyte secondary battery, and battery pack

A non-aqueous electrolyte secondary battery with specific electrode body dimensions, confining pressure, and electrolyte composition stabilizes LiFSO3, addressing output resistance and capacity retention issues during high-rate cycling.

JP2024160471AActive Publication Date: 2024-11-14PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023075495
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14
Estimated Expiration
2043-05-01

AI Technical Summary

Technical Problem

Repetitive high-rate charging and discharging of LiFSO-containing non-aqueous electrolyte secondary batteries leads to deteriorated battery characteristics, including increased output resistance and decreased capacity retention rate.

Method used

The battery design incorporates a wound or laminated electrode body with specific dimensions and a confining pressure of 0.5 MPa or more, using an electrolyte with LiFSO3 and a conductivity of 0.86 S/m or more, optionally supplemented with LiPF6 and LiBF4, and a solvent mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate, to maintain electrolyte stability and suppress transition metal elution.

Benefits of technology

The solution effectively reduces output resistance and maintains capacity retention rate even after repeated high-rate charging and discharging by preventing positive electrode active material reactions and transition metal elution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160471000001
    Figure 2024160471000001
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery that can reduce the output resistance and suppress the decrease in capacity retention.SOLUTION: A nonaqueous electrolyte secondary battery includes an electrode body and an electrolyte solution. The electrode body is a wound electrode body or a stack electrode body including a positive electrode plate containing an active material layer. The length of the active material layer in a direction parallel to a winding axis of the wound electrode body is 150 mm or more. The shape of the stack electrode body in a plan view is a square or a rectangle, and the length of the active material layer in a direction parallel to one side of the square or a direction parallel to a long side of the rectangle is 150 mm or more. In the nonaqueous electrolyte secondary battery, a restraint pressure of 0.5 MPa or more is applied in a lamination direction of the positive electrode plate. The electrolyte solution contains LiFSO3 and has an electric conductivity of 0.86 S / m or more at 25°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous electrolyte secondary battery and a battery pack. [Background technology]

[0002] It is known that LiFSO3 is used as an electrolyte for non-aqueous electrolyte secondary batteries. For example, Patent Document 1 discloses that the initial charge capacity, input / output characteristics, and internal impedance characteristics of the battery are improved by using an electrolyte containing LiPF6 and LiFSO3. Patent Document 2 discloses that practically sufficient conductivity can be obtained by adjusting the composition of the non-aqueous electrolyte. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-152956 A [Patent Document 2] JP 2014-170730 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, it has been found that repeated high-rate charging and discharging of batteries using an electrolyte containing LiFSO3 leads to a decrease in battery characteristics.

[0005] The present disclosure aims to provide a nonaqueous electrolyte secondary battery and a battery pack that can reduce output resistance and suppress a decrease in capacity retention rate even when high-rate charging and discharging are repeated using an electrolyte solution containing LiFSO3. [Means for solving the problem]

[0006] [1] A nonaqueous electrolyte secondary battery including an electrode assembly and an electrolyte solution, The electrode body is a wound type electrode body or a laminated type electrode body including a positive electrode plate having an active material layer, When the electrode body is a wound type electrode body, the length of the active material layer in a direction parallel to the winding axis is 150 mm or more, When the electrode body is a laminated electrode body, The laminated electrode body has a square or rectangular shape in a plan view, a length of the active material layer in a direction parallel to one side of the square or a direction parallel to a long side of the rectangle is 150 mm or more; The nonaqueous electrolyte secondary battery is applied with a confining pressure of 0.5 MPa or more in a stacking direction of the positive electrode plate, The electrolyte contains LiFSO3, The electrolytic solution has an electrical conductivity of 0.86 S / m or more at 25° C. [2] The nonaqueous electrolyte secondary battery according to [1], wherein the content of LiFSO3 in the electrolyte is 0.1% by mass or more and 2.5% by mass or less. [3] The nonaqueous electrolyte secondary battery according to [1] or [2], wherein the electrolytic solution has an electrical conductivity of 0.90 S / m or more at 25° C. [4] The nonaqueous electrolyte secondary battery according to any one of [1] to [3], wherein the electrolytic solution has an electrical conductivity of 0.93 S / m or more at 25° C. [5] The nonaqueous electrolyte secondary battery according to any one of [1] to [4], wherein the electrolyte solution further contains at least one of LiPF6 and LiBF4. [6] The nonaqueous electrolyte secondary battery according to any one of [1] to [5], wherein the electrolyte solution further contains vinylene carbonate. [7] The nonaqueous electrolyte secondary battery according to any one of [1] to [6], wherein the electrolytic solution further contains one or more selected from the group consisting of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate. [8] A battery pack in which two or more batteries are arranged so as to be electrically connected, the battery is a non-aqueous electrolyte secondary battery including an electrode assembly and an electrolyte solution, The electrode body is a wound type electrode body or a laminated type electrode body including a positive electrode plate having an active material layer, When the electrode body is a wound type electrode body, the length of the active material layer in a direction parallel to the winding axis is 150 mm or more, When the electrode body is a laminated electrode body, The laminated electrode body has a square or rectangular shape in a plan view, a length of the active material layer in a direction parallel to one side of the square or a direction parallel to a long side of the rectangle is 150 mm or more; The electrolyte contains LiFSO3, The electrolytic solution has an electrical conductivity of 0.86 S / m or more at 25° C.; The battery pack is constrained so that a constraining pressure of 0.5 MPa or more is applied in a stacking direction of the positive electrode plates of the batteries. Effect of the Invention

[0007] The nonaqueous electrolyte secondary battery of the present disclosure can reduce output resistance and suppress a decrease in capacity retention rate even when repeatedly charged and discharged at high rates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] (Nonaqueous electrolyte secondary battery) The nonaqueous electrolyte secondary battery of this embodiment (hereinafter also referred to as "the present battery (1)") includes an electrode body and an electrolyte. The electrode body includes a positive electrode plate having a positive electrode active material layer (active material layer), and is a wound electrode body or a laminated electrode body. When the electrode body is a wound electrode body, the length of the positive electrode active material layer in a direction parallel to the winding axis is 150 mm or more. When the electrode body is a laminated electrode body, the planar shape of the laminated electrode body is a square or rectangle, and the length of the positive electrode active material layer in a direction parallel to one side of the square or a direction parallel to the long side of the rectangle is 150 mm or more. In the present battery (1), a confining pressure of 0.5 MPa or more is applied in the stacking direction of the positive electrode plate. The electrolyte contains LiFSO3, and the electrical conductivity of the electrolyte at 25 ° C. is 0.86 S / m or more.

[0009] The electrode assembly usually includes a positive electrode plate, a negative electrode plate, and a separator. The negative electrode plate includes a negative electrode active material layer including a negative electrode active material. The separator is interposed between the positive electrode plate and the negative electrode plate.

[0010] When the electrode body is a wound electrode body, the length of the positive electrode active material layer and the negative electrode active material layer in the direction parallel to the winding axis may be independently 150 mm or more, 150 mm or more and 350 mm or less, 180 mm or more and 350 mm or less, or 200 mm or more and 300 mm or less. When the electrode body is a laminated electrode body whose planar shape is square or rectangular, the length of the positive electrode active material layer and the negative electrode active material layer in the direction parallel to one side of the square, or the length of the positive electrode active material layer and the negative electrode active material layer in the direction parallel to the long side of the rectangle may be independently 150 mm or more, 150 mm or more and 350 mm or less, 180 mm or more and 350 mm or less, or 200 mm or more and 300 mm or less. In the electrode body, the length of both the positive electrode active material layer and the negative electrode active material layer is preferably within the above-mentioned range.

[0011] The confining pressure applied to the battery (1) may be 0.5 MPa or more in the stacking direction of the positive electrode plates. The stacking direction of the positive electrode plates is usually the same direction as the stacking direction of the positive electrode plates and the negative electrode plates. The confining pressure may be 0.5 MPa or more and 5 MPa or less, 1 MPa or more and 4 MPa or less, or 2 MPa or more and 4 MPa or less. The confining pressure can be calculated by measuring the load using a load cell. The confining pressure applied to the battery (1) may be applied in a state in which the battery (1) is assembled into an assembled battery. A method for assembling the assembled battery includes a method for assembling the battery (2) described later into an assembled battery.

[0012] The electrolyte is usually a non-aqueous electrolyte, preferably a non-aqueous solvent such as an organic solvent containing a supporting salt. The electrolyte contains LiFSO3. The content of LiFSO3 in the electrolyte is preferably 0.1% by mass or more and 2.5% by mass or less, may be 0.5% by mass or more and 2.0% by mass or less, or may be 0.7% by mass or more and 1.5% by mass or less. The content of LiFSO3 in the electrolyte is the amount of LiFSO3 relative to the total amount of the electrolyte.

[0013] Examples of supporting salts that may be included in the electrolytic solution include LiPF6, LiBF4, LiClO4, and LiBOB (lithium bis(oxalato)borate), in addition to the above-mentioned LiFSO3. The electrolytic solution may contain one or more of these. In addition to LiFSO3, the electrolytic solution preferably contains a supporting salt other than LiFSO3, more preferably contains at least one of LiPF6 and LiBF4, and may contain LiPF6.

[0014] When the electrolyte contains at least one of LiPF6 and LiBF4, the concentration of LiPF6 and LiBF4 in the electrolyte is preferably 0.5 mol / L or more and 1.5 mol / L or less, and may be 0.7 mol / L or more and 1.4 mol / L or less, or may be 0.8 mol / L or more and 1.2 mol / L or less. The above concentration is the total number of moles of LiPF6 and LiBF4 per 1 L of non-aqueous solvent in the electrolyte. When the electrolyte contains one of LiPF6 and LiBF4, the above concentration is the concentration of the one, and when the electrolyte contains both LiPF6 and LiBF4, the concentration is the total concentration of LiPF6 and LiBF4.

[0015] Examples of non-aqueous solvents that may be included in the electrolytic solution include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), butylene carbonate (BC), and diethyl carbonate (DEC). The electrolytic solution may include one or more non-aqueous solvents among these. The electrolytic solution preferably includes one or more selected from the group consisting of EC, EMC, and DMC, and more preferably includes EC, EMC, and DMC.

[0016] When the non-aqueous solvent used in the electrolyte contains EC, DMC, and EMC, they may be contained in a mixing ratio of EC:DMC:EMC=5-50:10-70:10-70 (volume ratio), EC:DMC:EMC=10-40:20-60:20-60 (volume ratio), or EC:DMC:EMC=20-40:30-50:30-50 (volume ratio). In this specification, x to y (x and y are numerical values) indicate that x is equal to or greater than y and is equal to or less than y.

[0017] The electrolytic solution may further contain an additive. Examples of the additive include vinylene carbonate (VC), vinyl ethylene carbonate (VEC), and fluoroethylene carbonate. The electrolytic solution may contain one or more additives among these. The electrolytic solution preferably contains VC. The content of the additive in the electrolytic solution may be 0.1% by mass or more and 5% by mass or less, 0.5% by mass or more and 3% by mass or less, or 1% by mass or more and 2% by mass or less. The content of the additive in the electrolytic solution is the amount of the additive relative to the total amount of the electrolytic solution, and when two or more additives are contained, it is the total amount.

[0018] The electrical conductivity of the electrolyte at 25°C may be 0.86 S / m or more, may be 0.88 S / m or more, preferably 0.90 S / m or more, and more preferably 0.93 S / m or more. The electrical conductivity of the electrolyte at 25°C is not particularly limited, but may be 1.5 S / m or less, and may be 1.0 S / m or less. The electrical conductivity of the electrolyte can be adjusted by the type and content of the supporting salt contained in the electrolyte, and the type and composition of the non-aqueous solvent. The electrical conductivity of the electrolyte can be measured using an electrical conductivity meter in an environment of 25°C.

[0019] In a non-aqueous electrolyte secondary battery (hereinafter also referred to as a "secondary battery") in which the length of the active material layer is within the above range and the above-mentioned magnitude of confining pressure is applied, the salt concentration of the electrolyte is likely to vary depending on the position of the electrode assembly. Specifically, the salt concentration of the electrolyte is likely to be relatively small at the end of the electrode assembly. Therefore, when the secondary battery is repeatedly charged and discharged, the potential of the positive electrode plate increases at the end of the electrode assembly, and the positive electrode active material and FSO3 - When the potential of the positive plate reaches the reaction potential, the transition metal in the positive electrode active material dissolves, and the dissolved transition metal accumulates on the negative electrode plate. This is thought to result in a decrease in the capacity retention rate when the secondary battery is repeatedly charged and discharged at a high rate. In contrast, since the electrical conductivity of the electrolyte in this battery (1) is within the above-mentioned range, the potential of the positive plate does not easily increase, even when the battery is repeatedly charged and discharged, and the polarization of the positive plate is also suppressed. This is thought to result in a decrease in the capacity retention rate when the positive electrode active material and FSO3 - This suppresses the reaction with the transition metal and inhibits the elution of the transition metal in the positive electrode active material, so that even if the battery (1) is repeatedly charged and discharged at a high rate, the decrease in capacity retention rate can be inhibited.

[0020] As described above, the electrode assembly may have, for example, a positive electrode plate, a negative electrode plate, and a separator. The electrode assembly is housed in an outer casing, and an electrolyte is poured into the outer casing that houses the electrodes. The opening of the outer casing into which the electrolyte is poured is sealed with a sealing plate.

[0021] The positive electrode plate can have a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode current collector is, for example, a metal foil made of an aluminum material such as aluminum or an aluminum alloy. The positive electrode active material layer contains a positive electrode active material. Examples of the positive electrode active material include layered or spinel-based lithium transition metal oxides (e.g., LiNiCoMnO2, LiNiO2, LiCoO2, LiFeO2, LiMn2O4, LiNi 0.5 Mn 1.5 O4, LiCrMnO4, LiFePO4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) are examples.

[0022] The positive electrode active material layer may contain one or both of a binder and a conductive assistant in addition to the positive electrode active material. Examples of the binder include styrene butadiene rubber (SBR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE). Examples of the conductive assistant include carbon materials such as fibrous carbon, carbon black (acetylene black, ketjen black, etc.), coke, and activated carbon. Examples of the fibrous carbon include carbon nanotubes (hereinafter also referred to as "CNTs"). The CNTs may be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes such as double-walled carbon tubes (DWCNTs).

[0023] The negative electrode plate may have a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode current collector is, for example, a metal foil made of a copper material such as copper or a copper alloy. The negative electrode active material layer includes a negative electrode active material. Examples of the negative electrode active material include a carbon-based active material containing a carbon (C) atom such as graphite; and a metal-based active material containing a metal element such as a metal oxide or a metal element containing an element selected from the group consisting of silicon (Si), tin (Sn), antimony (Sb), bismuth (Bi), titanium (Ti), and germanium (Ge). The negative electrode active material layer may include a Si-based active material containing a silicon element as a metal-based active material.

[0024] Examples of the Si-based active material include silicon alone, SiC (a composite material of silicon and carbon, for example, silicon nanoparticles dispersed in porous carbon particles), SiOx, LixSiyOz, etc. The Si-based active material expands and contracts greatly with charging and discharging, and the salt concentration of the electrolyte is likely to vary when the battery is repeatedly charged and discharged at a high rate. Since the present battery (1) has an electrolyte with an electrical conductivity within the above-mentioned range, it has a negative electrode active material containing a Si-based active material, and is considered to be able to suppress a decrease in the capacity retention rate even when the battery is repeatedly charged and discharged at a high rate.

[0025] The negative electrode active material layer may contain one or both of a binder and a conductive assistant in addition to the negative electrode active material. Examples of the binder include cellulose-based binders such as carboxymethyl cellulose (CMC), methyl cellulose (MC), and hydroxypropyl cellulose; styrene butadiene rubber (SBR), polyacrylic acid (PAA), acrylonitrile butadiene rubber (NBR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE). Examples of the conductive assistant include those mentioned above.

[0026] The separator may be a porous sheet (film, nonwoven fabric, etc.) made of a resin such as polyethylene, polypropylene, polyester, cellulose, or polyamide. The porous sheet may have a single-layer structure or a multi-layer structure of two or more layers. The separator may have a functional layer on the surface of the porous sheet. The functional layer may be at least one of a heat-resistant layer and an adhesive layer for bonding to a positive electrode plate and a negative electrode plate.

[0027] The exterior body is a housing that houses the electrode assembly and has an opening for housing the electrode assembly. The opening of the exterior body can be sealed with a sealing plate. The exterior body and the sealing plate are preferably made of metal and can be formed using aluminum, an aluminum alloy, iron, an iron alloy, or the like, and can be formed using, for example, an aluminum laminate film.

[0028] (Battery pack) The battery pack of this embodiment is a battery pack in which two or more batteries are arranged so as to be electrically connected. The battery pack includes a non-aqueous electrolyte secondary battery (hereinafter also referred to as "the present battery (2)") and includes an electrode body and an electrolytic solution. The electrode body is a wound electrode body or a laminated electrode body including a positive electrode plate having an active material layer. When the electrode body is a wound electrode body, the length of the positive electrode active material layer in a direction parallel to the winding axis is 150 mm or more. When the electrode body is a laminated electrode body, the laminated electrode body has a square or rectangular shape in a plan view, and the length of the positive electrode active material layer in a direction parallel to one side of the square or in a direction parallel to the long side of the rectangle is 150 mm or more. The electrolytic solution includes LiFSO3, and the electrical conductivity of the electrolytic solution at 25°C is 0.86 S / m or more. The battery pack is constrained so that a constraining pressure of 0.5 MPa or more is applied in the stacking direction of the positive electrode plates of the present battery (2).

[0029] The electrode assembly and electrolyte contained in the present battery (2) may be those described as the electrode assembly and electrolyte contained in the present battery (1). The electrode assembly and electrolyte are usually housed in the above-mentioned exterior body, and the opening of the exterior body is sealed with a sealing plate. The length of the positive electrode active material layer, the length of the negative electrode active material layer, and the electrical conductivity of the electrolyte may be within the ranges described for the present battery (1).

[0030] A battery pack typically comprises two or more batteries (2) arranged adjacent to each other in the stacking direction of the positive electrodes of the batteries (2), and the batteries (2) are arranged so that the stacking directions of the positive electrodes of the batteries (2) are the same.

[0031] The confining pressure of the battery pack may be 0.5 MPa or more and 5 MPa or less, 1 MPa or more and 4 MPa or less, or 2 MPa or more and 4 MPa or less. The confining pressure can be calculated by measuring the load with a load cell. The confining pressure of the battery pack is preferably set so that a confining pressure of 0.5 MPa or more is applied to the battery (2) in the stacking direction of the positive electrode plates. The confining pressure applied to the battery (2) may be 0.5 MPa or more and 5 MPa or less, 1 MPa or more and 4 MPa or less, or 2 MPa or more and 4 MPa or less.

[0032] The battery (2) included in the assembled battery may be the battery (1). For example, the assembled battery may be two or more batteries (1) arranged so as to be electrically connected. In this case, the assembled battery is configured by arranging two or more batteries (1) adjacent to each other in the stacking direction of the positive electrode plates of the batteries (1), and the batteries (1) may be arranged so that the stacking directions of the positive electrode plates of the batteries (1) are the same. The confining pressure applied to the batteries (1) may be a confining pressure applied when the batteries (1) are assembled into the assembled battery. EXAMPLES

[0033] The present disclosure will be described more specifically below with reference to examples, comparative examples, and reference examples. Comparative Example 1 (Preparation of positive electrode plate) LiNiCoMnO2 as a positive electrode active material, acetylene black (AB) as a conductive assistant, and polyvinylidene fluoride (PVdF) as a binder were used in a ratio of LiNiCoMnO2:AB:pVdF=100:1:1 (mass ratio), which was mixed with N-methylpyrrolidone (NMP) to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied to an aluminum foil as a positive electrode current collector, dried, and compressed to a predetermined thickness to form a positive electrode active material layer on the aluminum foil, and then cut out to a predetermined width to obtain a positive electrode plate. The positive electrode plate had, in the width direction, a region where the positive electrode active material layer was formed on the aluminum foil and a region where the positive electrode active material layer was not formed and the aluminum foil was exposed. The width of the positive electrode active material layer of the positive electrode plate (the length in the direction parallel to the winding axis of the electrode body described later) was 150 mm.

[0034] (Preparation of negative electrode plate) Graphite as the negative electrode active material, styrene butadiene rubber (SBR) as the binder, and carboxymethyl cellulose (CMC) were used in a ratio of graphite:SBR:CMC=100:1:1 (mass ratio), and this was mixed with water to obtain a negative electrode mixture slurry. The negative electrode mixture slurry was applied to a copper foil as a negative electrode current collector, dried, and compressed to a predetermined thickness to form a negative electrode active material layer on the copper foil, and then cut out to a predetermined width to obtain a negative electrode plate. The negative electrode plate had, in the width direction, a region where the negative electrode active material layer was formed on the copper foil and a region where the negative electrode active material layer was not formed and the copper foil was exposed. The width of the negative electrode active material layer of the negative electrode plate (the length in the direction parallel to the winding axis of the electrode body described later) was 155 mm.

[0035] (Preparation of electrode body) A separator having a three-layer structure of polypropylene / polyethylene / polypropylene was prepared. The positive and negative plates obtained above were laminated and wound with the separator interposed therebetween to obtain a wound electrode body. The wound electrode body had a positive current collector exposed at one end in a direction parallel to the winding axis, and a negative current collector exposed at the other end. An aluminum plate for external current collection was welded to the area where the positive current collector of the wound electrode body was exposed, and a copper plate for external current collection was welded to the area where the negative current collector was exposed, and then the wound electrode body was housed in an exterior body formed of an aluminum laminate film.

[0036] A comparative electrolyte (1) was prepared by mixing LiPF6, VC, and the mixed solvent, using LiPF6 as the supporting salt and a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) (EC:EMC:DMC=30:50:20 (volume ratio)) as the non-aqueous solvent, so that the concentration of LiPF6 was 1.1 mol / L and the content of vinylene carbonate (VC) as an additive was 1 mass%. This comparative electrolyte (1) was poured into an exterior housing containing a wound electrode body, and the opening of the exterior housing was sealed with a sealing plate to obtain an assembly.

[0037] In the assembly, stainless steel restraining plates were placed on each of the two faces parallel to the winding axis of the wound electrode body (i.e., the two faces perpendicular to the lamination direction of the positive and negative electrode plates of the wound electrode body), and the assembly was sandwiched between the two restraining plates. The four corners of the two restraining plates were fastened to each other using bolts and nuts, and the load was adjusted so that a restraining pressure of 0.5 MPa was applied to the assembly, thereby obtaining a nonaqueous electrolyte secondary battery. The restraining pressure can be calculated by measuring the load with a load cell.

[0038] Comparative Example 2 A comparative electrolyte (2) was prepared in the same manner as the comparative electrolyte (1), except that LiPF6 and LiFSO3 were used as supporting electrolytes, the LiPF6 concentration was 1.1 mol / L, the LiFSO3 content was 1 mass%, and the VC content was 1 mass%. A nonaqueous electrolyte secondary battery was obtained in the same manner as the comparative example 1, except that the comparative electrolyte (2) was used instead of the comparative electrolyte (1).

[0039] [Comparative Example 3, Examples 1 to 4] Comparative electrolyte solution (3) and electrolyte solutions (1) to (4) were prepared in the same manner as comparative electrolyte solution (2), except that a mixed solvent of EC, EMC, and DMC was used in the mixing ratio shown in Table 1. A nonaqueous electrolyte secondary battery was obtained in the same manner as comparative example 1, except that comparative electrolyte solution (3) and electrolyte solutions (1) to (4) were used instead of comparative electrolyte solution (1).

[0040] Comparative Example 4 A comparative electrolyte solution (4) was prepared in the same manner as the comparative electrolyte solution (1), except that a mixed solvent of EC:EMC:DMC=30:30:40 (volume ratio) was used. A nonaqueous electrolyte secondary battery was obtained in the same manner as in Comparative Example 1, except that the comparative electrolyte solution (4) was used instead of the comparative electrolyte solution (1).

[0041] [Examples 5 and 6] Electrolyte solutions (5) and (6) were prepared in the same manner as for the electrolyte solution (3) of Example 3, except that LiFSO3 was used so as to have the content shown in Table 1. Non-aqueous electrolyte secondary batteries were obtained in the same manner as for Comparative Example 1, except that the electrolyte solutions (5) and (6) were used instead of the comparative electrolyte solution (1).

[0042] Comparative Example 5 A nonaqueous electrolyte secondary battery was obtained in the same manner as in Example 3, except that no confining pressure was applied.

[0043] [Reference example 1] A wound electrode body was obtained in the same manner as in Comparative Example 1, except that the width of the positive electrode active material layer of the positive electrode plate (the length in the direction parallel to the winding axis of the electrode body) was changed to 100 mm, and the width of the negative electrode active material layer of the negative electrode plate (the length in the direction parallel to the winding axis of the electrode body) was changed to 103 mm. A nonaqueous electrolyte secondary battery was obtained using this wound electrode body.

[0044] [Reference example 2] A wound electrode body was obtained in the same manner as in Comparative Example 2, except that the width of the positive electrode active material layer of the positive electrode plate (the length in the direction parallel to the winding axis of the electrode body) was changed to 100 mm, and the width of the negative electrode active material layer of the negative electrode plate (the length in the direction parallel to the winding axis of the electrode body) was changed to 103 mm. A nonaqueous electrolyte secondary battery was obtained using this wound electrode body.

[0045] [Measurement of electrical conductivity] The electrical conductivity of the electrolyte was measured in a thermostatic chamber at 25° C. using an electrical conductivity meter (manufactured by Toa DKK Co., Ltd.).

[0046] <Evaluation> (Initial activation) In an environment of 25° C., the nonaqueous electrolyte secondary battery obtained above was charged to 4.2 Vcccv (constant current / constant voltage) at a current value of C / 10, and stored for 24 hours at 60° C. After that, the battery was discharged to a potential of 3 V at a current value of C / 10, thereby performing initial activation of the nonaqueous electrolyte secondary battery.

[0047] [Evaluation of output resistance] The initially activated non-aqueous electrolyte secondary battery was charged at a current value of C / 3 in an environment of 25° C. until the SOC (charge rate) reached 50%, and then rested for 30 minutes, after which the voltage V0 of the non-aqueous electrolyte secondary battery was measured. Then, in an environment of 25° C., the battery was discharged for 10 seconds at a current value of 2C, and the voltage V1 of the non-aqueous electrolyte secondary battery at the 10th second was measured. The resistance of the non-aqueous electrolyte secondary battery was calculated according to the following formula. Resistance [Ω] = (V0-V1) / 2C current value

[0048] The resistance values ​​of Comparative Examples 2 to 5 and Examples 1 to 6 were converted as relative values ​​when the resistance value of Comparative Example 1 was set to 100% (reference). The resistance value of Reference Example 2 was converted as a relative value when the resistance value of Reference Example 1 was set to 100% (reference). The results are shown in Table 1.

[0049] [Cycle test] In a thermostatic chamber at 25°C, the initially activated non-aqueous electrolyte secondary battery was charged to 4.2Vcccv (constant current / constant voltage) at a current value of 2C, and then discharged to a potential of 3V at a current value of 1C. This cycle was repeated. The retention rate of the discharge capacity W500 at the 500th cycle relative to the discharge capacity W1 at the 1st cycle was calculated as the capacity retention rate [%] according to the following formula. The results are shown in Table 1. Capacity maintenance rate [%]=(W500 / W1)×100

[0050] [Table 1]

[0051] In Comparative Example 2, in which an electrolyte solution containing LiFSO3 was used, the output resistance was reduced compared to Comparative Example 1, in which an electrolyte solution not containing LiFSO3 was used, but the capacity retention rate was also reduced. In Comparative Example 2, the output resistance was reduced by including LiFSO3, but the positive electrode active material and FSO3 - It is presumed that the capacity retention rate decreased due to a reaction between the positive electrode active material and the transition metal in the positive electrode active material being eluted.

[0052] A comparison of Comparative Example 3 with Examples 1 to 4 shows that the smaller the volume ratio (EMC / DMC) of EMC and DMC in the mixed solvent, the higher the electrical conductivity, the lower the output resistance, and the better the capacity retention rate. A comparison of Comparative Example 4 with Examples 5 and 6 shows that the higher the content of LiFSO3 in the mixed solvent, the lower the output resistance and the better the capacity retention rate. The inclusion of LiFSO3 can reduce the output resistance, and the higher the electrical conductivity of the electrolyte, the better the interaction between the positive electrode active material and FSO3 during high-rate charging. - It is believed that the capacity retention rate could be improved because the reaction with the cathode was suppressed, and the elution of the transition metal in the positive electrode active material was suppressed.

[0053] It is considered that in Comparative Example 5 where no confining pressure was applied, the inter-electrode distance was larger, resulting in a larger output resistance, compared to Example 3 where confining pressure was applied. Therefore, it is considered that in Comparative Example 3, the reversibility of Li ions was deteriorated, and the capacity retention rate was also deteriorated, compared to Example 3.

[0054] In Reference Examples 1 and 2, the width of the positive electrode active material layer is smaller than in Comparative Examples 1 and 2. Comparison between Reference Example 2 and Comparative Example 2 shows that when the width of the positive electrode active material layer is small, the salt concentration of the electrolyte is less likely to vary, and the positive electrode active material and FSO3 - It is considered that the reaction with the transition metal in the positive electrode active material is unlikely to occur, and therefore the transition metal in the positive electrode active material is unlikely to be eluted. Therefore, it is presumed that the capacity retention rate of Reference Example 2 is improved compared to Comparative Example 2.

Claims

1. A non-aqueous electrolyte secondary battery including an electrode assembly and an electrolyte solution, The electrode body is a wound type electrode body or a laminated type electrode body including a positive electrode plate having an active material layer, When the electrode body is a wound type electrode body, the length of the active material layer in a direction parallel to a winding axis is 150 mm or more, When the electrode body is a laminated electrode body, The laminated electrode body has a square or rectangular shape in a plan view, a length of the active material layer in a direction parallel to one side of the square or a direction parallel to a long side of the rectangle is 150 mm or more; The nonaqueous electrolyte secondary battery is applied with a confining pressure of 0.5 MPa or more in a stacking direction of the positive electrode plate, The electrolyte is LiFSO 3 Including, The electrolytic solution has an electrical conductivity of 0.86 S / m or more at 25° C.

2. LiFSO in the electrolyte 3 The nonaqueous electrolyte secondary battery according to claim 1 , wherein the content of is 0.1% by mass or more and 2.5% by mass or less.

3. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrolytic solution has an electrical conductivity of 0.90 S / m or more at 25°C.

4. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrolytic solution has an electrical conductivity of 0.93 S / m or more at 25°C.

5. The electrolyte further contains LiPF 6 and LiBF 4 The nonaqueous electrolyte secondary battery according to claim 1 , further comprising at least one of:

6. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrolyte further contains vinylene carbonate.

7. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrolytic solution further contains at least one selected from the group consisting of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate.

8. A battery pack in which two or more batteries are arranged so as to be electrically connected, the battery is a non-aqueous electrolyte secondary battery including an electrode assembly and an electrolyte solution, The electrode body is a wound type electrode body or a laminated type electrode body including a positive electrode plate having an active material layer, When the electrode body is a wound type electrode body, the length of the active material layer in a direction parallel to a winding axis is 150 mm or more, When the electrode body is a laminated electrode body, The laminated electrode body has a square or rectangular shape in a plan view, a length of the active material layer in a direction parallel to one side of the square or a direction parallel to a long side of the rectangle is 150 mm or more; The electrolyte is LiFSO 3 Including, The electrolytic solution has an electrical conductivity of 0.86 S / m or more at 25° C.; The battery pack is constrained such that a constraining pressure of 0.5 MPa or more is applied in a stacking direction of the positive electrode plates of the batteries.

Citation Information

Patent Citations

  • Battery structure

    JP2007311264A

  • Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

    JP2013152956A

  • Nonaqueous electrolyte secondary battery and manufacturing method

    JP2016143454A

  • Lithium ion secondary battery

    JP2017033827A

  • Lithium ion secondary battery and battery pack

    JP2018032575A