Glass for chemical strengthening, chemically strengthened glass, electronic device and method for producing chemically strengthened glass

A chemically strengthened glass with specific oxide ratios and a two-stage ion exchange process enhances electrical resistance, effectively suppressing abnormal light emission in electronic devices by increasing compressive stress layers, addressing the issue of electrostatic charging in organic EL displays.

JP2024160696APending Publication Date: 2024-11-14AGC INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024071340
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-04-25
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The occurrence of abnormal light emission phenomena in electronic devices, particularly in organic EL displays, is attributed to electrostatic charging, which existing chemically strengthened glass compositions fail to adequately address.

Method used

A chemically strengthened glass composition with specific oxide ratios and ion exchange treatments, including a two-stage ion exchange process using molten salt compositions, enhances electrical resistance to suppress abnormal light emission by increasing the depth and amount of compressive stress layers.

Benefits of technology

The proposed glass composition effectively suppresses abnormal light emission in electronic devices by ensuring high electrical resistance through controlled ion exchange, resulting in chemically strengthened glass with improved durability and resistance to electrostatic charging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160696000001_ABST
    Figure 2024160696000001_ABST
Patent Text Reader

Abstract

To provide glass for chemical strengthening and chemically strengthened glass which, when used in cover glass for displays in electronic devices and the like, prevents abnormal light emission phenomena in the displays.SOLUTION: The present invention provides glass for chemical strengthening with a specific compositional range, where the ratio of the total content of Li2O, Na2O and K2O to the content of Al2O3 (R2O / Al2O3) satisfies formula (A) 0.8≤(R2O / Al2O3)≤30, and chemically strengthened glass with K-DOL of 4.2 μm or more, or K-CSarea of 4000 Pa m or more, as defined by below, and a surface resistivity of 11 [logΩ / sq] or more. K-CS0(MPa): the compressive stress value at the glass surface, measured with a glass surface stress meter, K-DOL(μm): the depth value of the compressive stress layer induced by potassium ions from the glass surface, K-CSarea(Pa m): the product of K-CS0 and K-DOL.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to glass for chemical strengthening, chemically strengthened glass, an electronic device, and a method for producing chemically strengthened glass. [Background technology]

[0002] Chemically strengthened glass is used for cover glass of mobile terminals, etc. Chemically strengthened glass is made by contacting glass with a molten salt composition such as sodium nitrate to cause ion exchange between alkali metal ions contained in the glass and alkali metal ions having a larger ionic radius than those contained in the molten salt composition, thereby forming a compressive stress layer on the surface of the glass.

[0003] Patent Document 1 discloses that the lower the surface resistivity of a chemically strengthened cover glass, the higher the durability of the antifouling layer formed on the cover glass. The surface resistivity is correlated with the electrical conductivity of the glass surface, and a low surface resistivity indicates a high electrical conductivity of the glass surface. In other words, increasing the electrical conductivity of the glass surface improves the durability of the antifouling layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021 / 010376 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a problem with mobile devices and other electronic devices where a part of the organic light-emitting diode (OLED) display emits light continuously and unintentionally. This phenomenon is thought to be related to static electricity caused by rubbing the display for a long period of time.

[0006] Patent Document 1 focuses on the relationship between the surface resistivity of chemically strengthened glass and the adhesion of an antifouling layer formed on the surface, but makes no consideration of the abnormal luminescence phenomenon.

[0007] An object of the present invention is to provide a glass for chemical strengthening and a chemically strengthened glass that can suppress abnormal light emission in a display when used as a cover glass for a display of an electronic device or the like. [Means for solving the problem]

[0008] The inventors of the present invention believe that the anomalous luminescence phenomenon is related to the tendency of charge transfer to occur due to electrostatic charging, and have found that the electrical resistance of glass (hereinafter sometimes simply referred to as "resistance") is related to the tendency of the anomalous luminescence phenomenon to occur. More specifically, they have found that the relatively higher the electrical resistance of glass is, the easier it is to suppress the anomalous luminescence phenomenon, and have thus completed the present invention.

[0009] That is, the present disclosure relates to the following: 1. Mole percentage based on oxides. SiO2 50% or more, B2O3 0-10% Al2O3 1-30%, P2O5 0-10%, Y2O3 0-10%, Li2O 0~25%, Na2O 0-25%, K2O 0-25%, MgO 0-10%, CaO 0-10%, SrO 0-10%, BaO 0-10%, ZnO 0-10%, ZrO2 0-5%, TiO2 0-5%, SnO2 0-5%, Fe2O3 content 0-0.5% A glass for chemical strengthening, in which the ratio (R2O / Al2O3) of the total content of Li2O, Na2O, and K2O to the content of Al2O3 satisfies the following formula (A): (A) 0.8≦(R2O / Al2O3)≦30 2. Mole percentage based on oxides. Li2O 7~12%, Na2O 1.5-6%, 2. The glass for chemical strengthening according to 1 above, containing 0 to 1.5% of K2O. 3. The K-DOL defined below is 4.2 μm or more, and Chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions 4. The K-CSarea defined below is 4000 Pa m or more, and Chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. K-CSarea(Pa m): Product of K-CS0 and K-DOL K-CS0 (MPa): Compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions 5. The chemically strengthened glass according to 4 above, wherein the K-CSO is 800 MPa or more. 6. The ratio of the K2O concentration at a depth of 3 μm from the glass surface (K2O@3 μm) to the K2O concentration at the center of the sheet thickness (K2O@center) is 5.3 or more; Chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. 7. The ratio of the Li2O concentration at a depth of 5 μm from the glass surface (Li2O@5μm) to the Li2O concentration at the center of the plate thickness (Li2O@center) is 0.85 or less; Chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. 8. The chemically strengthened glass according to any one of 3 to 7 above, wherein the value of Y defined below is 9.4 or more. Y=0.00018x1+4.319×10 -7 x2+8.5 x1: Product of K-CS0 and K-DOL K-CSarea (Pa m) x2: Product of Na-CS0 and Na-DOL Na-CSarea (Pa m) K-CS0 (MPa): Compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions Na-CS0 (MPa): Compressive stress value on the glass surface measured with a scattered light photoelastic stress meter Na-DOL (μm): The depth from the glass surface of the compressive stress layer caused by sodium ions 9. An electronic device comprising the chemically strengthened glass according to 1 or 2 above or the chemically strengthened glass according to any one of 3 to 8 above. 10. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising: a second ion exchange treatment in which, after the first ion exchange treatment, the glass for chemical strengthening is brought into contact with a second molten salt composition, 2. A method for producing chemically strengthened glass, wherein the second molten salt composition has a KNO3 content of 94 mass % or more and a lithium ion content of less than 300 mass ppm. 11. The method for producing chemically strengthened glass according to item 10, wherein the temperature of the second molten salt composition in the second ion exchange treatment is 380°C to 450°C, and the time for which the second molten salt composition is brought into contact with the glass for chemical strengthening is 60 minutes or longer. 12. The method for producing chemically strengthened glass according to claim 10 or 11, wherein the second molten salt composition contains 0 to 5 mass % of NaNO3. 13. A method for producing chemically strengthened glass, comprising subjecting glass for chemical strengthening to an ion exchange treatment to obtain chemically strengthened glass, The K-DOL defined below is 4.2 μm or more, and A method for producing chemically strengthened glass, which produces chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions 14. A method for producing chemically strengthened glass, comprising subjecting glass for chemical strengthening to an ion exchange treatment to obtain chemically strengthened glass, The K-CSarea defined below is 4000 Pa m or more, and A method for producing chemically strengthened glass, which produces chemically strengthened glass with a surface resistivity of 11 [log Ω / sq] or more. K-CSarea(Pa m): Product of CS0 and K-DOL CS0 (MPa): Compressive stress value on the glass surface K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions Effect of the Invention

[0010] According to the present invention, it is possible to provide a chemically strengthened glass that can suppress the abnormal light emission phenomenon of a display when used as a cover glass for a display of an electronic device, etc. Also, it is possible to provide a glass for chemical strengthening that can easily obtain a chemically strengthened glass having high resistance by chemical strengthening. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram for explaining the abnormal light emission phenomenon. [Diagram 2] FIG. 2 is a diagram showing the relationship between surface resistivity and volume resistivity. [Diagram 3] FIG. 3 is a diagram showing the relationship between the value of Y and the volume resistivity (actual measured value). [Figure 4] FIG. 4 shows the K2O profile of the surface layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In this specification, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits. In addition, in this specification, the composition of the glass (content of each component) is expressed in mole percentage based on oxides, and mole % is simply expressed as "%", unless otherwise specified. In addition, in this specification, "substantially free" means that the content is below the impurity level contained in raw materials, that is, that it is not intentionally added. Specifically, for example, it is less than 0.1%.

[0013] In this specification, "amorphous glass" refers to glass that does not show diffraction peaks indicating crystals by powder X-ray diffraction. "Crystallized glass" is obtained by heating "amorphous glass" to precipitate crystals, and contains crystals. In this specification, "amorphous glass" and "crystallized glass" are sometimes collectively referred to as "glass." In addition, amorphous glass that becomes crystallized glass by heat treatment is sometimes referred to as "mother glass of crystallized glass." In the following, "chemically strengthened glass" refers to glass after chemical strengthening treatment, and "glass for chemical strengthening" refers to glass before chemical strengthening treatment.

[0014] <Stress measurement method> In recent years, glass that has been chemically strengthened in two or more stages has become mainstream for use in cover glass for devices such as smartphones. In this process, the lithium ions inside the glass are first exchanged for sodium ions (Li-Na exchange), and then the sodium ions on the surface of the glass are further exchanged for potassium ions (Na-K exchange).

[0015] In order to obtain such a stress profile of chemically strengthened glass in a non-destructive manner, for example, a scattered light photoelastic stress meter (hereinafter also abbreviated as SLP) or a film stress measurement (hereinafter also abbreviated as FSM) can be used in combination.

[0016] The method using a scattered light photoelastic stress meter (SLP) can measure the compressive stress due to Li-Na exchange in the glass interior at a depth of several tens of micrometers from the glass surface.

[0017] On the other hand, a method using a glass surface stress meter (FSM) can measure the compressive stress resulting from Na-K exchange in the surface layer of the glass, within a few tens of μm from the glass surface (for example, WO 2018 / 056121, WO 2017 / 115811).

[0018] Therefore, in two-stage chemically strengthened glass, a combination of SLP and FSM information is sometimes used as the stress profile in the glass surface and interior.

[0019] In the present invention, the stress profile measured mainly by a scattered light photoelastic stress meter (SLP) is used. In this specification, the compressive stress CS, the tensile stress CT, the compressive stress layer depth DOC, etc. refer to the values ​​in the SLP stress profile.

[0020] The scattered light photoelastic stress meter is a stress measuring device having a polarization phase difference variable member that varies the polarization phase difference of laser light by one or more wavelengths relative to the wavelength of the laser light, an imaging element that captures the scattered light emitted when the laser light with the varied polarization phase difference is incident on strengthened glass multiple times at a specified time interval to obtain multiple images, and a calculation unit that uses the multiple images to measure the periodic luminance change of the scattered light, calculates the phase change of the luminance change, and calculates the stress distribution in the depth direction from the surface of the strengthened glass based on the phase change.

[0021] A method for measuring a stress profile using a scattered light photoelastic stress meter includes the method described in International Publication No. 2018 / 056121. Examples of the scattered light photoelastic stress meter include SLP-1000 and SLP-2000 manufactured by Orihara Seisakusho. High-precision stress measurement is possible by combining these scattered light photoelastic stress meters with the attached software SlpIV_up3 (Ver.2019.01.10.001).

[0022] <K-DOL、K-CS0、K-CSarea> In this specification, "K-DOL" refers to the depth of the compressive stress layer caused by potassium ions, which originates from Na-K exchange, in the glass surface layer within a few tens of μm from the glass surface. K-DOL is a value that can be approximated by the depth at which the potassium ion concentration becomes equal to the potassium ion concentration at the center of the plate thickness. It can also be measured as the measurement limit value of the compressive stress layer depth measured by a glass surface stress meter (FSM). "K-CS0" is the compressive stress value caused by potassium ions at a depth of 0 μm measured by FSM. "K-CSarea" is the product of K-CS0 and K-DOL.

[0023] <Na-DOL、Na-CS0、Na-CSarea> In this specification, "Na-DOL" refers to the depth of a compressive stress layer caused by Na ions, which is derived from Li-Na exchange, in the glass interior at a depth of several tens of μm or more from the glass surface. Na-DOL is the depth at which the magnitude of the compressive stress generated by Na ions becomes zero. "Na-CS0" is the compressive stress value caused by Na ions at a depth of 0 μm measured by SLP. "Na-CSarea" is the product of Na-CS0 and Na-DOL.

[0024] <ctave> "CTave" (MPa) in this specification is determined by the following formula. CTave corresponds to the average value of the tensile stress, which is the value obtained by integrating the stress values in the tensile stress region and dividing by the length of the tensile stress region. CTave = ICT / L CT ICT: Integral value of tensile stress (Pa·m) L CT : Thickness direction length of the tensile stress region (μm)

[0025] <CS x > "CS" in this specification x " is the compressive stress value (MPa) at a depth x (μm) from the glass surface. This numerical value is the value measured by SLP.

[0026] <K2O concentration, Na2O concentration> In this specification, the K2O concentration and Na2O concentration at a depth x (μm) are measured by EPMA (Electron Probe Micro Analyzer) for the concentration in the cross-section in the thickness direction. The measurement by EPMA is specifically performed as follows, for example.

[0027] First, embed the glass sample in an epoxy resin, and prepare a cross-section sample by mechanically polishing it in a direction perpendicular to the first main surface and the second main surface facing the first main surface. Apply a C coat to the polished cross-section and perform the measurement using EPMA (manufactured by JEOL: JXA - 8500F). The acceleration voltage is 15 kV, the probe current is 30 nA, and the integration time is 1000 msec. / point. Obtain the line profile of the X-ray intensity of K2O or Na2O at 1-μm intervals. For the obtained K2O concentration profile or Na2O concentration profile, calculate the total thickness count by proportional conversion to mol% with the average count in the central part of the thickness (0.5 × t) ± 25 μm (where the thickness is t μm) as the population composition.

[0028] <Li2O concentration> In this specification, the Li2O concentration at a depth x (μm) is measured at a cross section in the plate thickness direction by GD-OES (Glow Discharge Optical Emission Spectroscopy). Specifically, the GD-OES measurement is performed, for example, as follows. First, the glass sample is cleaned by washing. Measurements are performed using a Marcus-type high-frequency glow discharge optical emission analyzer (HORIBA Seisakusho, GD-Profiler2). The emission spectrum is obtained against the sputtering time under the following conditions: discharge conditions 40 W (constant power mode), Ar pressure 200 Pa, discharge mode pulse sputtering mode (duty cycle 0.25DS), and discharge range 4 mmφ. The obtained Li concentration is normalized with the concentration in the unreinforced substrate and then converted proportionally to the Li2O concentration contained in the substrate. The discharge mark depth after measurement is measured with a surface roughness meter, and the sputtering time is converted to the measured depth in 0.00025 μm increments. The profile is then smoothed using the centered moving average method with a width of 0.25 μm.

[0029] <Chemically strengthened glass> Chemical strengthening is a process in which glass is brought into contact with a metal salt (e.g., sodium nitrate or potassium nitrate) containing a metal ion with a large ionic radius (typically, sodium ion or potassium ion) by a method such as immersion in, coating or spraying in a melt of the metal salt, and metal ions with a small ionic radius (typically, lithium ion or sodium ion) in the glass are replaced with metal ions with a large ionic radius in the metal salt (typically, sodium ion or potassium ion for lithium ion, and potassium ion for sodium ion).

[0030] <Relationship between anomalous luminescence and electrical resistance of glass> As mentioned above, there is a problem with electronic devices such as mobile terminals where a part of the display unintentionally emits light continuously, which is called an "abnormal light emission phenomenon." This phenomenon is known to occur particularly in PI-OLEDs (organic electroluminescence displays using a polyimide substrate). It is known that the abnormal light emission phenomenon can typically occur after rubbing the display of an electronic device with a finger for an extended period of time. The light emission is said to be more likely to occur near the edge (periphery) or hole of the display, and the light emission is said to last for a long time (up to 1-2 days in some cases) rather than a short time.

[0031] The inventors have also found that, in order to suppress the anomalous luminescence phenomenon, it is effective to make the electrical resistance of the glass used for the cover glass relatively high. Based on this, the inventors have found that the electrical resistance of chemically strengthened glass can be made relatively high by a chemical strengthening process, and that chemically strengthened glass with high electrical resistance can be easily obtained by adjusting the glass composition within an appropriate range, and have completed the present invention.

[0032] In this specification, the electrical resistance of the cover glass is evaluated by surface resistivity or volume resistivity. Here, surface resistivity is the resistivity per 1 cm 2 It is the value of surface resistance per cm2 of glass. The surface resistivity of a certain principal surface of glass correlates with the ease of movement of electric charges in a direction parallel to the principal surface direction, and the higher the surface resistivity, the more difficult it is for electric charges to flow in a direction parallel to the principal surface direction. Therefore, the surface resistivity is a value that has almost no correlation with the thickness of the glass. Also, the volume resistivity is the value of the surface resistivity per cm2 of glass. 3 The volume resistivity of glass correlates with the ease of movement of electric charges between one main surface of the glass and the other main surface facing it (hereinafter sometimes simply referred to as the thickness direction), and the higher the volume resistivity, the more difficult it is for electric charges to flow in the thickness direction.

[0033] FIG. 2 shows the relationship between the surface resistivity and the volume resistivity of chemically strengthened glass when a plate-shaped glass for chemical strengthening having the same matrix composition and plate thickness is subjected to a chemical strengthening process under a number of different conditions. From this figure, it can be seen that the chemical strengthening process can affect the electrical resistance of chemically strengthened glass. In other words, it can be seen that the electrical resistance of chemically strengthened glass can be increased by appropriately controlling the conditions of the chemical strengthening process or the properties of the chemically strengthened glass obtained thereby. Furthermore, as a result of the study by the present inventors, it is considered that the following cases (I) and (II) contribute to increasing the electrical resistance of chemically strengthened glass. (I) In the vicinity of the glass surface, a plurality of different alkali metal ions are present in a more mixed state in nearly equal proportions. (II) In the vicinity of the glass surface, a larger number of alkali metal ions, which are relatively large, are introduced by the chemical strengthening treatment.

[0034] In addition, from FIG. 2, it can be seen that there is a positive correlation between the surface resistivity and the volume resistivity. When the surface vicinity of the chemically strengthened glass is relatively highly resistive and an electric charge moves in a direction parallel to the main surface direction, the electric charge is difficult to move near the surface of the main surface, and the electric charge is considered to bypass the relatively deep part from the main surface. In this case, when the surface resistivity is measured, the electric charge is considered to pass through the high resistance part twice when moving from the vicinity of the main surface to the deep part and when returning from the deep part to the vicinity of the main surface. Similarly, when measuring the volume resistivity, the electric charge is considered to pass through the high resistance part twice by passing through the high resistance part near one main surface and the high resistance part near the other main surface. From these, it can be explained that there is a linear positive correlation between the surface resistivity and the volume resistivity. From these, it can be said that according to the chemically strengthened glass with a relatively high resistance, the movement of the electric charge can be suppressed in both the direction parallel to the display main surface and the plate thickness direction, which contributes to the suppression of the abnormal light emission phenomenon.

[0035] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments, and can be modified as desired without departing from the scope of the present invention. For example, among the embodiments exemplified in this specification, preferred aspects of each embodiment can be combined with each other, or a part of each embodiment can be replaced with a preferred aspect of another embodiment.

[0036] The glass for chemical strengthening of the present embodiment includes glasses for chemical strengthening of a first embodiment and a second embodiment described below.

[0037] (First embodiment) The glass for chemical strengthening according to the first embodiment of the present invention is In terms of mole percentage based on oxide, SiO2 50% or more, B2O3 0-10% Al2O3 1-30%, P2O5 0-10%, Y2O3 0-10%, Li2O 0~25%, Na2O 0-25%, K2O 0-25%, MgO 0-10%, CaO 0-10%, SrO 0-10%, BaO 0-10%, ZnO 0-10%, ZrO2 0-5%, TiO2 0-5%, SnO2 0-5%, Fe2O3 content 0-0.5% The ratio (R2O / Al2O3) of the total content of Li2O, Na2O, and K2O to the content of Al2O3 satisfies the following formula (A). (A) 0.8≦(R2O / Al2O3)≦30

[0038] Since the chemically strengthened glass according to the first embodiment has the above composition, the glass itself tends to have a relatively high resistance, and when chemically strengthened, it is easy to obtain chemically strengthened glass with high resistance.

[0039] The glass for chemical strengthening according to the first embodiment preferably contains, in terms of mole percentages based on oxides, 7 to 12% LiO, 1.5 to 6% NaO, and 0 to 1.5% KO, from the viewpoints of increasing the surface resistivity and volume resistivity and of introducing into the glass a compressive stress necessary for improving the strength of the glass.

[0040] Hereinafter, a more preferred composition of the glass for chemical strengthening according to the first embodiment will be described in detail. In the glass composition, the lower limit of the content of non-essential components is preferably 0%.

[0041] In the chemically strengthened glass according to this embodiment, SiO2 is a component that forms a network structure of the glass and also increases the chemical durability. The SiO2 content is 50% or more, preferably 52% or more, more preferably 56% or more, even more preferably 60% or more, particularly preferably 64% or more, and most preferably 68% or more. On the other hand, in order to improve the melting property, the SiO2 content is less than 75%, preferably 73% or less, more preferably 72% or less, even more preferably 71% or less, particularly preferably 70% or less, and most preferably 69% or less.

[0042] B2O3 is a component that improves the chipping resistance of the chemically strengthened glass or the chemically strengthened glass and improves the meltability, and may be contained. When B2O3 is contained, the content is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more in order to improve the meltability. On the other hand, if the content of B2O3 is too high, striae may occur during melting, or phase separation may occur easily, which may lead to a deterioration in the quality of the chemically strengthened glass, so that the content is preferably 10% or less. The content of B2O3 is more preferably 8% or less, even more preferably 6% or less, and particularly preferably 4% or less.

[0043] Al2O3 is an essential component that increases the surface compressive stress due to chemical strengthening. The content of Al2O3 is 1% or more, and is preferably 3% or more, 5% or more, 7% or more, 9% or more, 11% or more, more preferably 12% or more, even more preferably 13% or more, particularly preferably 14% or more, and most preferably 15% or more. On the other hand, the content of Al2O3 is 30% or less so that the devitrification temperature of the glass does not become too high, and is preferably 27% or less, more preferably 24% or less, even more preferably 21% or less, particularly preferably 19% or less, and most preferably 18% or less.

[0044] P2O5 is not essential, but may be contained since it is a component that increases the compressive stress layer due to chemical strengthening. In addition, since P2O5 is a component that can promote the diffusion of potassium ions during chemical strengthening treatment, it is preferable to contain P2O5 from the viewpoint of obtaining chemically strengthened glass with high resistance. P2O5 is also a component that can promote crystallization in crystallized glass. When P2O5 is contained, the content is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, if the P2O5 content is too high, phase separation occurs easily when melted and acid resistance is significantly reduced, so the P2O5 content is 10% or less, preferably 8% or less, more preferably 6% or less, even more preferably 5% or less, particularly preferably 4% or less, and most preferably 3% or less.

[0045] Y2O3 is not essential, but is an ingredient that has the effect of preventing the chemically strengthened glass from scattering into pieces when broken, and may be contained. When Y2O3 is contained, the content is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, in order to suppress devitrification during melting, the Y2O3 content is 10% or less, preferably 8% or less, more preferably 6% or less, even more preferably 4% or less, particularly preferably 3.5% or less, and most preferably 3% or less.

[0046] Li2O, Na2O and K2O are components that have the effect of increasing the surface resistivity and volume resistivity, and the effect of adjusting the ion exchange properties of the glass in order to appropriately introduce a compressive stress required for improving the strength of the glass into the glass. In the present embodiment, the total content of Li2O, Na2O and K2O is more than 0% from the viewpoint of increasing the surface resistivity and volume resistivity, and from the viewpoint of introducing a compressive stress by chemical strengthening treatment, and is preferably 10% or more, more preferably 11% or more, even more preferably 12% or more, particularly preferably 14% or more, and most preferably 16% or more. The total content of Li2O, Na2O and K2O is preferably 35% or less, more preferably 30% or less, even more preferably 25% or less, particularly preferably 20% or less, and most preferably 19% or less from the viewpoint of reducing the devitrification properties during glass molding.

[0047] In the glass according to this embodiment, the ratio (R2O / Al2O3) of the total content of Li2O, Na2O, and K2O to the content of Al2O3 satisfies the following formula (A). (A) 0.8≦(R2O / Al2O3)≦30 When (R2O / Al2O3) satisfies the above formula (A), it means that the content of Al2O3 is relatively high or low compared to the content of alkali metal oxides, which has the effect of increasing the surface resistivity and volume resistivity.

[0048] When (R2O / Al2O3) satisfies the above formula (A), (R2O / Al2O3) is 0.8 or more, preferably 0.84 or more, more preferably 0.88 or more, even more preferably 0.92 or more, particularly preferably 0.96 or more, and most preferably 1.0 or more. On the other hand, (R2O / Al2O3) is 30 or less, and is preferably 25 or less, 20 or less, 10 or less, 5 or less, 2 or less, more preferably 1.8 or less, even more preferably 1.5 or less, and even more preferably 1.0 or less.

[0049] Li2O is a component that generates compressive stress through ion exchange. Li2O is not essential, but when it is contained, the content is preferably 3% or more, more preferably 5% or more, even more preferably 7% or more, even more preferably 8% or more, particularly preferably 9% or more, and most preferably 10% or more. On the other hand, in order to stabilize the glass, the content of Li2O is 25% or less, preferably 22% or less, more preferably 20% or less, even more preferably 18% or less, particularly preferably 16% or less, even more particularly preferably 14% or less, and most preferably 12% or less.

[0050] Na2O is a component that improves the meltability of glass. Na2O is not essential, but when it is contained, the content is preferably 1% or more, more preferably 1.5% or more, even more preferably 2% or more, even more preferably 3% or more, particularly preferably 4% or more, and most preferably 5% or more. If Na2O is too much, the chemical strengthening properties are reduced, so the Na2O content is preferably 25% or less, more preferably 20% or less, even more preferably 15% or less, particularly preferably 12% or less, even more particularly preferably 10% or less, and most preferably 6% or less.

[0051] K2O is not essential, but like Na2O, it is a component that lowers the melting temperature of glass and may be contained. When K2O is contained, the content is preferably 0.1% or more, more preferably 0.5% or more, even more preferably 1% or more, particularly preferably 1.5% or more, and most preferably 2% or more. If the amount of K2O is too much, the chemical strengthening properties or chemical durability decreases, so the content is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, particularly preferably 5% or less, even more particularly preferably 4% or less, and most preferably 1.5% or less.

[0052] The total content of Na2O and K2O (Na2O+K2O) is preferably 2% or more, more preferably 3% or more, even more preferably 4% or more, particularly preferably 5% or more, and most preferably 6% or more in order to improve the meltability of the glass raw material. Na2O+K2O is preferably 20% or less, more preferably 15% or less, even more preferably 12% or less, particularly preferably 10% or less, and most preferably 8% or less.

[0053] BaO, SrO, MgO, CaO and ZnO are all components that improve the melting property of glass and may be contained. When any one or more of BaO, SrO, MgO, CaO and ZnO are contained, the total content of these is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, from the viewpoint of keeping the ion exchange rate at a certain level or higher, the total content of these is preferably 10% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0054] Although MgO is not essential, it is a component that stabilizes the glass and also enhances the mechanical strength and chemical resistance, and therefore, when the Al2O3 content is relatively low, it is preferable to contain MgO. The MgO content is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, if too much MgO is added, the viscosity of the glass decreases and devitrification or phase separation is likely to occur. The content of MgO is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0055] CaO is not essential, but is a component that improves the meltability of glass and may be contained. The CaO content is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, if the CaO content is excessive, it becomes difficult to increase the compressive stress value during chemical strengthening treatment. The CaO content is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0056] SrO is not essential, but is a component that improves the meltability of glass and may be contained. The SrO content is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, if the SrO content is excessive, it becomes difficult to increase the compressive stress value during chemical strengthening treatment. The SrO content is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0057] BaO is not essential, but is a component that improves the meltability of glass and may be contained. The BaO content is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, if the BaO content is excessive, it becomes difficult to increase the compressive stress value during chemical strengthening treatment. The BaO content is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0058] ZnO is not essential, but is a component that improves the meltability of glass and may be contained. The ZnO content is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, if the ZnO content is excessive, it becomes difficult to increase the compressive stress value during chemical strengthening treatment. The ZnO content is 10% or less, preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, particularly preferably 6% or less, and most preferably 5% or less.

[0059] ZrO2 is not essential, but is a component that enhances mechanical strength and chemical durability and significantly improves CS, so its inclusion is preferred. The ZrO2 content is preferably 0.2% or more, more preferably 0.5% or more, further preferably 1% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, in order to suppress devitrification during melting, the ZrO2 content is preferably 5% or less, more preferably 4.7% or less, more preferably 4.4% or less, even more preferably 4% or less, particularly preferably 3.7% or less, and most preferably 3.5% or less.

[0060] TiO2 is not essential, but it is a component that suppresses the solarization of glass, and also promotes crystallization when obtaining crystallized glass, so it may be contained. When TiO2 is contained, the content is preferably 0.1% or more, more preferably 0.5% or more, even more preferably 1% or more, particularly preferably 1.5% or more, and most preferably 2% or more. On the other hand, in order to suppress devitrification during melting, the content of TiO2 is preferably 5% or less, more preferably 4.7% or less, more preferably 4.4% or less, even more preferably 4% or less, particularly preferably 3.7% or less, and most preferably 3.5% or less.

[0061] Although SnO2 is not essential, it may be contained since it acts as a clarifier during glass production and also promotes the formation of crystal nuclei when obtaining crystallized glass. When SnO2 is contained, the content is preferably 0.02% or more, more preferably 0.05% or more, even more preferably 0.08% or more, particularly preferably 0.1% or more, and most preferably 0.12% or more. On the other hand, in order to suppress devitrification during melting, the content of SnO2 is preferably 5% or less, more preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, particularly preferably 0.5% or less, and most preferably 0.3% or less.

[0062] La2O3, Nb2O5 and Ta2O5 are all components that make it difficult for chemically strengthened glass to scatter fragments when broken, and may be contained to increase the refractive index. When these are contained, the total content of La2O3, Nb2O5 and Ta2O5 (hereinafter, La2O3+Nb2O5+Ta2O5) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. In addition, in order to make the glass less susceptible to devitrification during melting, La2O3+Nb2O5+Ta2O5 is preferably 4% or less, more preferably 3% or less, even more preferably 2% or less, and particularly preferably 1% or less.

[0063] CeO2 may also be contained. CeO2 may suppress coloring by oxidizing the glass. When CeO2 is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and even more preferably 0.07% or more. In order to increase transparency, the content of CeO2 is preferably 1.5% or less, and more preferably 1.0% or less.

[0064] When chemically strengthened glass is used after coloring, coloring components may be added to the extent that the desired chemical strengthening characteristics are not hindered. Examples of coloring components include Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, Er2O3, and Nd2O3.

[0065] When Fe2O3 is contained, its content is 0.5% or less. The total content of coloring components is preferably 1% or less. If it is desired to increase the visible light transmittance of the glass, it is preferable that these components are substantially not contained.

[0066] In order to improve weather resistance against ultraviolet light irradiation, HfO2, Nb2O5, and Ti2O3 may be added. When added for the purpose of improving weather resistance against ultraviolet light irradiation, the total content of HfO2, Nb2O5, and Ti2O3 is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.1% or less, in order to suppress the influence on other properties.

[0067] In addition, SO3, chlorides, and fluorides may be appropriately contained as clarifiers for melting glass. The total content of components functioning as clarifiers is preferably 2% or less, more preferably 1% or less, and even more preferably 0.5% or less, expressed as mass% on an oxide basis, since adding too much of them affects the strengthening characteristics and crystallization behavior. The lower limit is not particularly limited, but typically, the total content is preferably 0.05% or more, expressed as mass% on an oxide basis.

[0068] When SO3 is used as a fining agent, the content of SO3 is preferably 0.01% or more, more preferably 0.05% or more, and even more preferably 0.1% or more, expressed as mass% on the oxide basis, since the effect is not observed if the content is too small. Also, when SO3 is used as a fining agent, the content of SO3 is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass% on the oxide basis.

[0069] When Cl is used as a fining agent, if too much is added, it affects physical properties such as strengthening characteristics, so the Cl content is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less, expressed as mass % on the oxide basis. Also, if Cl is used as a fining agent, if the Cl content is too low, no effect is observed, so the Cl content is preferably 0.05% or more, more preferably 0.1% or more, and even more preferably 0.2% or more, expressed as mass % on the oxide basis.

[0070] It is preferable that As2O3 is not contained. When As2O3 is contained, the content is preferably 0.3% or less, more preferably 0.1% or less, and most preferably, As2O3 is not contained.

[0071] The glass for chemical strengthening according to the first embodiment may be amorphous glass or crystallized glass.

[0072] Second embodiment The glass for chemical strengthening according to the second embodiment of the present invention preferably has a matrix composition, expressed in mole % on an oxide basis, of 40 to 70% SiO2, 10 to 35% Li2O, and 1 to 15% Al2O3.

[0073] One aspect of the glass for chemical strengthening according to the second embodiment is, in mole percent on an oxide basis, SiO2 40-70%, Li2O 10~35%, Al2O3 1-15%, P2O5 0.5-5%, ZrO2 0.5-5%, B2O3 0-10%, Na2O 0-3%, K2O 0-1%, It is preferable that the glass contains 0 to 4% of SnO2. In this specification, the crystallized glass having such a composition is also referred to as "the present crystallized glass x".

[0074] Another aspect of the glass for chemical strengthening according to the second embodiment is, in mole percent on an oxide basis, SiO2 50-70%, Li2O 15~30%, Al2O3 1-10%, P2O5 0.5-5%, ZrO2 0.5-8%, MgO 0.1-10%, Y2O3 0-5% B2O3 0-10%, Na2O 0-3%, K2O 0-1%, It is preferable that the glass contains 0 to 2% of SnO2. In this specification, the crystallized glass having such a composition is also referred to as "the present crystallized glass y."

[0075] In this specification, the crystallized glass of the present embodiment including the crystallized glass x and the crystallized glass y is also collectively referred to as the crystallized glass of the present embodiment. The crystallized glass of the present embodiment is preferably 60 to 80% in total amount of SiO2, Al2O3, P2O5 and B2O3 in mole percent based on oxide. SiO2, Al2O3, P2O5 and B2O3 are glass network forming components (hereinafter also abbreviated as NWF). The strength of glass increases when the total amount of these NWFs is large. This increases the fracture toughness value of the crystallized glass, so the total amount of NWF is preferably 60% or more, more preferably 63% or more, and particularly preferably 65% ​​or more. However, glass with too much NWF has a high melting temperature and is difficult to manufacture, so the total amount is preferably 85% or less, more preferably 80% or less, and more preferably 75% or less.

[0076] In the present crystallized glass, the ratio of the total amount of Li2O, Na2O and K2O to the NWF, that is, the total amount of SiO2, Al2O3, P2O5 and B2O3, is preferably 0.20 to 0.60.

[0077] Li2O, Na2O and K2O are network modifiers, and decreasing the ratio to NWF increases the gaps in the network, improving impact resistance. Therefore, the ratio of the total amount of Li2O, Na2O and K2O to NWF is preferably 0.60 or less, more preferably 0.55 or less, and particularly preferably 0.50 or less. On the other hand, since these are necessary components for chemical strengthening, in order to improve the chemical strengthening properties, the ratio of the total amount of Li2O, Na2O and K2O to NWF is preferably 0.20 or more, more preferably 0.25 or more, and particularly preferably 0.30 or more. The glass composition will be described below.

[0078] In the present amorphous glass, SiO2 is a component that forms a network structure of glass. It is also a component that increases chemical durability, and the SiO2 content is preferably 45% or more. The SiO2 content is more preferably 48% or more, even more preferably 50% or more, particularly preferably 52% or more, and extremely preferably 54% or more. On the other hand, in order to improve melting property, the SiO2 content is preferably 70% or less, more preferably 68% or less, even more preferably 66% or less, and particularly preferably 64% or less.

[0079] Al2O3 is a component that increases the surface compressive stress due to chemical strengthening, and is essential. The content of Al2O3 is preferably 1% or more, more preferably 2% or more, further preferably 3% or more, 5% or more, 5.5% or more, 6% or more, particularly preferably 6.5% or more, and most preferably 7% or more. On the other hand, the content of Al2O3 is preferably 15% or less, more preferably 12% or less, further preferably 10% or less, particularly preferably 9% or less, and most preferably 8% or less, so that the devitrification temperature of the glass does not become too high.

[0080] Li2O is a component that forms surface compressive stress by ion exchange, and is essential because it is a component of the main crystal. The content of Li2O is preferably 10% or more, more preferably 14% or more, more preferably 15% or more, even more preferably 18% or more, particularly preferably 20% or more, and most preferably 22% or more. On the other hand, in order to stabilize the glass, the content of Li2O is preferably 35% or less, more preferably 32% or less, even more preferably 30% or less, particularly preferably 28% or less, and most preferably 26% or less.

[0081] Na2O is a component that improves the melting property of glass. Na2O is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 1% or more, and particularly preferably 2% or more. If there is too much Na2O, it becomes difficult to precipitate crystals such as Li3PO4, which is the main crystal, or the chemical strengthening properties are reduced, so the content of Na2O is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, and particularly preferably 7% or less.

[0082] K2O is a component that lowers the melting temperature of glass like Na2O, and may be contained. When K2O is contained, the content is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. If the amount of K2O is too much, the chemical strengthening properties or chemical durability will decrease, so the content is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less.

[0083] The total content of Na2O and K2O, Na2O+K2O, is preferably 1% or more, and more preferably 2% or more, in order to improve the meltability of the glass raw materials.

[0084] In addition, the ratio of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O) is preferably 0.2 or less, since this improves the chemical strengthening properties and chemical durability. K2O / R2O is more preferably 0.15 or less, and even more preferably 0.10 or less.

[0085] R2O is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. R2O is preferably 29% or less, and more preferably 26% or less.

[0086] P2O5 is a component of Li3PO4 crystal and is essential. The content of P2O5 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and extremely preferably 2.5% or more in order to promote crystallization. On the other hand, if the content of P2O5 is too high, phase separation occurs easily during melting and acid resistance is significantly reduced, so the content of P2O5 is preferably 5% or less, more preferably 4.8% or less, even more preferably 4.5% or less, and particularly preferably 4.2% or less.

[0087] ZrO2 is a component that enhances mechanical strength and chemical durability, and is preferably contained because it significantly improves CS. The content of ZrO2 is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more. On the other hand, in order to suppress devitrification during melting, ZrO2 is preferably 8% or less, more preferably 7.5% or less, even more preferably 7% or less, and particularly preferably 6% or less. If the content of ZrO2 is too high, the viscosity decreases due to an increase in the devitrification temperature. In order to suppress deterioration of moldability due to such a decrease in viscosity, when the molding viscosity is low, the content of ZrO2 is preferably 5% or less, more preferably 4.5% or less, and even more preferably 3.5% or less.

[0088] In order to improve chemical durability, ZrO2 / R2O is preferably 0.02 or more, more preferably 0.03 or more, even more preferably 0.04 or more, particularly preferably 0.1 or more, and most preferably 0.15 or more. In order to improve transparency after crystallization, ZrO2 / R2O is preferably 0.6 or less, more preferably 0.5 or less, even more preferably 0.4 or less, and particularly preferably 0.3 or less.

[0089] Since MgO is a component that stabilizes glass and also enhances mechanical strength and chemical resistance, it is preferable to contain it when the Al2O3 content is relatively low. The content of MgO is preferably 1% or more, more preferably 2% or more, even more preferably 3% or more, and particularly preferably 4% or more. On the other hand, if too much MgO is added, the viscosity of the glass decreases and devitrification or phase separation is likely to occur, so the content of MgO is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, and particularly preferably 7% or less.

[0090] TiO2 is a component that can promote crystallization and may be contained. TiO2 is not essential, but if it is contained, it is preferably 0.2% or more, more preferably 0.5% or more. On the other hand, in order to suppress devitrification during melting, the content of TiO2 is preferably 4% or less, more preferably 2% or less, and even more preferably 1% or less.

[0091] SnO2 has the effect of promoting the formation of crystal nuclei and may be contained. SnO2 is not essential, but when it is contained, it is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. On the other hand, in order to suppress devitrification during melting, the content of SnO2 is preferably 6% or less, more preferably 5% or less, even more preferably 4% or less, and particularly preferably 3% or less.

[0092] Y2O3 is a component that has the effect of preventing fragments from scattering when the chemically strengthened glass is broken, and may be contained. The content of Y2O3 is preferably 1% or more, more preferably 1.5% or more, even more preferably 2% or more, particularly preferably 2.5% or more, and extremely preferably 3% or more. On the other hand, in order to suppress devitrification during melting, the content of Y2O3 is preferably 5% or less, more preferably 4% or less.

[0093] B2O3 is a component that improves the chipping resistance of the chemically strengthened glass or the chemically strengthened glass and improves the meltability, and may be contained. When B2O3 is contained, the content is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more in order to improve the meltability. On the other hand, if the content of B2O3 is too high, striae may occur during melting, or phase separation may occur easily, which may lead to a deterioration in the quality of the chemically strengthened glass, so that the content is preferably 5% or less. The content of B2O3 is more preferably 4% or less, even more preferably 3% or less, and particularly preferably 2% or less.

[0094] BaO, SrO, MgO, CaO and ZnO are all components that improve the melting property of glass and may be contained. When these components are contained, the total content of BaO, SrO, MgO, CaO and ZnO (hereinafter, BaO+SrO+MgO+CaO+ZnO) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. On the other hand, since the ion exchange rate decreases, BaO+SrO+MgO+CaO+ZnO is preferably 8% or less, more preferably 6% or less, even more preferably 5% or less, and particularly preferably 4% or less.

[0095] Among these, BaO, SrO, and ZnO may be contained to improve the refractive index of the residual glass and bring it closer to the precipitated crystal phase, thereby improving the light transmittance of the crystallized glass and reducing the haze value. In this case, the total content of BaO, SrO, and ZnO (hereinafter, BaO+SrO+ZnO) is preferably 0.3% or more, more preferably 0.5% or more, even more preferably 0.7% or more, and particularly preferably 1% or more. On the other hand, these components may reduce the ion exchange rate. In order to improve the chemical strengthening properties, BaO+SrO+ZnO is preferably 2.5% or less, more preferably 2% or less, even more preferably 1.7% or less, and particularly preferably 1.5% or less.

[0096] La2O3, Nb2O5 and Ta2O5 are all components that make it difficult for chemically strengthened glass to scatter fragments when broken, and may be contained to increase the refractive index. When these are contained, the total content of La2O3, Nb2O5 and Ta2O5 (hereinafter, La2O3+Nb2O5+Ta2O5) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. In addition, in order to make the glass less susceptible to devitrification during melting, La2O3+Nb2O5+Ta2O5 is preferably 4% or less, more preferably 3% or less, even more preferably 2% or less, and particularly preferably 1% or less.

[0097] CeO2 may also be contained. CeO2 may suppress coloring by oxidizing the glass. When CeO2 is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and even more preferably 0.07% or more. In order to increase transparency, the content of CeO2 is preferably 1.5% or less, and more preferably 1.0% or less.

[0098] When the tempered glass is colored, a coloring component may be added to the glass within a range that does not impede the achievement of the desired chemical strengthening properties. Examples of the coloring component include Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, Er2O3, and Nd2O3.

[0099] The total content of coloring components is preferably within the range of 1% or less. If it is desired to increase the visible light transmittance of the glass, it is preferable that these components are substantially not contained.

[0100] In addition, SO3, chlorides, and fluorides may be appropriately contained as fining agents when melting the glass. It is preferable that As2O3 is not contained. When As2O3 is contained, it is preferably 0.3% or less, more preferably 0.1% or less, and most preferably not contained.

[0101] The glass for chemical strengthening according to the second embodiment is preferably glass-ceramic.

[0102] Here, when the chemically strengthened glass of the first and second embodiments is a crystallized glass, the composition of the crystal phase and the glass phase of the crystallized glass is preferably within the above-mentioned range. The composition of the crystallized glass is obtained by heat-treating the crystallized glass at a temperature above its melting point and analyzing the vitrified glass. The method for analyzing the glass composition includes fluorescent X-ray analysis.

[0103] When the chemically strengthened glass of the first and second embodiments is a crystallized glass, the crystal species is not particularly limited, but it is preferable to contain one or more crystals selected from the group consisting of lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals. As the lithium silicate crystals, lithium metasilicate crystals, lithium disilicate crystals, etc. are preferable. As the lithium phosphate crystals, lithium orthophosphate crystals, etc. are preferable. As the lithium aluminosilicate crystals, β-spodumene crystals, petalite crystals, etc. are preferable.

[0104] When the chemically strengthened glass of the first and second embodiments is a crystallized glass, the crystallization rate of the crystallized glass is not particularly limited, but is preferably 10% or more, more preferably 15% or more, even more preferably 20% or more, and particularly preferably 25% or more in order to increase the mechanical strength. Also, in order to increase the transparency, it is preferably 70% or less, more preferably 60% or less, and particularly preferably 50% or less. A small crystallization rate is also excellent in that it is easy to heat and bend. The crystallization rate can be calculated from the X-ray diffraction intensity by the Rietveld method. The Rietveld method is described in "Crystal Analysis Handbook" edited by the editorial committee of the Japanese Crystallographic Society (Kyoritsu Shuppan, 1999, p492-499).

[0105] The chemically strengthened glass of this embodiment includes the chemically strengthened glasses of the third to sixth embodiments described below.

[0106] Third embodiment The chemically strengthened glass according to the third embodiment of the present invention has a K-DOL defined below of 4.2 μm or more and a surface resistivity of 11 [log Ω / sq] or more. K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions

[0107] As described above, it is considered that chemically strengthened glass in which a compressive stress layer caused by potassium ions having a relatively large size is formed tends to have high resistance. Here, a relatively large K-DOL means that the depth of the compressive stress layer caused by potassium ions is relatively large. That is, according to the chemically strengthened glass of the third embodiment, a highly resistive compressive stress layer caused by potassium ions is formed deep, so that a chemically strengthened glass having a large surface resistivity is obtained.

[0108] In the chemically strengthened glass according to the third embodiment, the K-DOL is 4.2 μm or more, preferably 5.0 μm or more, more preferably 6.0 μm or more, even more preferably 8.0 μm or more, particularly preferably 10.0 μm or more, and most preferably 12.0 μm or more. On the other hand, from the viewpoint of maintaining high deep layer stress due to Na ions, the K-DOL is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, particularly preferably 18 μm or less, and most preferably 15 μm or less.

[0109] In the chemically strengthened glass according to the third embodiment, the surface resistivity is 11 [log Ω / sq] or more, preferably 11.5 [log Ω / sq] or more, and more preferably 12 [log Ω / sq] or more.

[0110] (Fourth embodiment) The chemically strengthened glass according to the fourth embodiment of the present invention has a K-CSarea defined below of 4000 Pa·m or more and a surface resistivity of 11 [log Ω / sq] or more. K-CSarea(Pa m): Product of K-CS0 and K-DOL K-CS0 (MPa): Compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions

[0111] As described above, it is considered that chemically strengthened glass in which a compressive stress layer caused by potassium ions having a relatively large size is formed tends to have a high resistance. Here, a relatively large K-CSarea means that the total amount of compressive stress caused by potassium ions is larger. That is, according to the chemically strengthened glass according to the fourth embodiment, the total amount of compressive stress caused by potassium ions is large, so that a chemically strengthened glass having a large surface resistivity is obtained.

[0112] In the chemically strengthened glass according to the fourth embodiment, K-CSarea is 4000 Pa·m or more, and in the following order, 4100 Pa·m or more, 4700 Pa·m or more, 5000 Pa·m or more are preferable, 6000 Pa·m or more are more preferable, and 10000 Pa·m or more are most preferable. On the other hand, from the viewpoint of keeping the deep layer stress due to Na ions high, K-CSarea is preferably 50000 Pa·m or less, more preferably 40000 Pa·m or less, even more preferably 30000 Pa·m or less, particularly preferably 20000 Pa·m or less, and most preferably 18000 Pa·m or less.

[0113] In the chemically strengthened glass according to the fourth embodiment, the surface resistivity is 11 [log Ω / sq] or more, preferably 11.5 [log Ω / sq] or more, and more preferably 12 [log Ω / sq] or more.

[0114] Fifth embodiment The chemically strengthened glass according to the fifth embodiment of the present invention has a ratio of K2O@3μm, which is the K2O concentration at a depth of 3μm from the glass surface, to K2O@center, which is the K2O concentration at the center of the plate thickness, of 5.3 or more, and has a surface resistivity of 11 [logΩ / sq] or more.

[0115] The ratio of K2O@3μm to K2O@center of 5.3 or more means that the total amount of potassium ions is relatively large in the range up to a depth of 3μm. That is, according to the chemically strengthened glass of the fifth embodiment, a high-resistance compressive stress layer caused by potassium ions is sufficiently formed, and a chemically strengthened glass with high surface resistivity is obtained.

[0116] In the chemically strengthened glass according to the fifth embodiment, the ratio of K2O@3μm to K2O@center is 5.3 or more, preferably 5.5 or more, more preferably 6.0 or more, and even more preferably 6.5 or more. On the other hand, from the viewpoint of keeping the deep layer stress due to Na ions high, this value is preferably 20 or less, more preferably 18 or less, even more preferably 15 or less, particularly preferably 12 or less, and most preferably 11 or less.

[0117] In the chemically strengthened glass according to the fifth embodiment, the surface resistivity is 11 [log Ω / sq] or more, preferably 11.5 [log Ω / sq] or more, and more preferably 12 [log Ω / sq] or more. The upper limit of the surface resistivity is not particularly limited.

[0118] Sixth embodiment The chemically strengthened glass according to the sixth embodiment of the present invention has a ratio of the Li2O concentration at a depth of 5 μm from the glass surface to the Li2O concentration at the center of the sheet thickness of 0.85 or less, and a surface resistivity of 11 [log Ω / sq] or more.

[0119] The ratio of Li2O@5μm, which is the Li2O concentration at a depth of 5μm from the glass surface, to Li2O@center, which is the Li2O concentration at the center of the plate thickness, being 0.85 or less means that the total amount of lithium ions in the range up to a depth of 5μm is relatively small. Lithium ions are relatively small in size among alkali metal ions. Therefore, when lithium ions are present in the surface layer of chemically strengthened glass, if other alkali metal ions are present in the vicinity, there is a possibility of high resistance due to the mixed alkali effect, but it is difficult to obtain the effect due to the size of the substituted alkali metal ions, and it is thought that it may work in the direction of lowering the resistance. In contrast, according to the chemically strengthened glass of the sixth embodiment, the amount of lithium ions contained in the surface layer is small, and the effect due to the size of the substituted alkali metal ions can be sufficiently obtained. As a result, a chemically strengthened glass having a high surface resistivity and a high resistance compressive stress layer is obtained.

[0120] In the chemically strengthened glass according to the sixth embodiment, the ratio of Li2O@5μm to Li2O@center is 0.85 or less, preferably 0.84 or less, more preferably 0.82 or less, even more preferably 0.80 or less, and most preferably 0.77 or less. On the other hand, from the viewpoint of improving the property of introducing Na ions deep into the glass by ion exchange, such a value is preferably 0 or more, more preferably 0.1 or more, even more preferably 0.2 or more, particularly preferably 0.3 or more, and most preferably 0.4 or more.

[0121] In the chemically strengthened glass according to the sixth embodiment, the surface resistivity is 11 [log Ω / sq] or more, preferably 11.5 [log Ω / sq] or more, and more preferably 12 [log Ω / sq] or more. The upper limit of the surface resistivity is not particularly limited.

[0122] In the chemically strengthened glass according to this embodiment, the value of Y defined below is preferably 9.4 or more. Y=0.000208x1+4.3×10 -7 x2+8.8 x1: Product of K-CS0 and K-DOL K-CSarea (Pa m) x2: Product of Na-CS0 and Na-DOL Na-CSarea (Pa m) K-CS0 (MPa): Compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): The depth from the glass surface of the compressive stress layer caused by potassium ions Na-CS0 (MPa): Compressive stress value on the glass surface measured with a scattered light photoelastic stress meter Na-DOL (μm): The depth from the glass surface of the compressive stress layer caused by sodium ions

[0123] FIG. 3 is a diagram showing the relationship between the value of Y and the measured value of volume resistivity of chemically strengthened glass in the examples of the present invention. As shown in FIG. 3, the inventors have found that the value of Y correlates well with the volume resistivity of chemically strengthened glass, and the larger the value of Y, the larger the volume resistivity of the chemically strengthened glass tends to be. That is, in this embodiment, a chemically strengthened glass with a large volume resistivity is obtained by making the value of Y relatively large. In order to increase the value of Y, it is effective to increase K-CSarea(x1) and Na-CSarea(x2), and it is particularly effective to increase x1.

[0124] The value of Y is preferably 9.4 or more, more preferably 9.6 or more, more preferably 9.8 or more, even more preferably 10 or more, even more preferably 10.3 or more, particularly preferably 10.6 or more, and most preferably 10.9 or more. There is no particular upper limit to the value of Y.

[0125] x1 represents the product K-CSarea (Pa·m) of K-CS0 and K-DOL. K-CSarea is preferably 4000 Pa·m or more, more preferably 4100 Pa·m or more, 4700 Pa·m or more, 5000 Pa·m or more, more preferably 6000 Pa·m or more, and particularly preferably 10000 Pa·m or more. On the other hand, from the viewpoint of keeping the deep stress due to Na ions high, K-CSarea is preferably 50000 Pa·m or less, more preferably 40000 Pa·m or less, even more preferably 30000 Pa·m or less, particularly preferably 20000 Pa·m or less, and most preferably 18000 Pa·m or less.

[0126] x2 represents the product Na-CSarea (Pa·m) of Na-CS0 and Na-DOL. From the viewpoint of increasing drop strength, when the thickness of the glass is t (mm), Na-CSarea is preferably (10000×t+1000) Pa·m or more, more preferably (10000×t+6000) Pa·m or more, even more preferably (10000×t+16000) Pa·m or more, particularly preferably (10000×t+26000) Pa·m or more, and most preferably (10000×t+31000) Pa·m or more. On the other hand, from the viewpoint of suppressing the stress in the glass to the tensile stress of the CT limit, Na-CSarea is preferably (140000×t+2000) Pa·m or less, more preferably (140000×t-8000) Pa·m or less, even more preferably (140000×t-18000) Pa·m or less, particularly preferably (140000×t-28000) Pa·m or less, and most preferably (140000×t-30000) Pa·m or less.

[0127] When a compressive stress layer is formed on the surface of a glass article, a tensile stress (hereinafter abbreviated as CT) corresponding to the total amount of compressive stress on the surface is inevitably generated in the center of the glass article. If this tensile stress value becomes too large, the glass article will break violently and fragments will scatter when it is broken. If the CT exceeds the threshold value (hereinafter abbreviated as CT limit), the number of fragments when damaged will increase explosively.

[0128] Therefore, chemically strengthened glass increases the compressive stress on the surface and forms a compressive stress layer in a deeper portion, while the total amount of compressive stress in the surface layer is designed so as not to exceed the CT limit (for example, U.S. Pat. No. 9,487,434, U.S. Patent Application Publication No. 2017 / 355640, U.S. Pat. No. 9,593,042, or JP2019-513663A).

[0129] (Chemically strengthened glass) More preferred aspects of the chemically strengthened glass according to each of the above embodiments include the following.

[0130] From the viewpoint of increasing bending strength, K-CSO (MPa) is preferably 800 MPa or more, more preferably 850 MPa or more, even more preferably 900 MPa or more, particularly preferably 950 MPa or more, and most preferably 1000 MPa or more.

[0131] From the viewpoint of increasing the drop strength, when the thickness of the glass is t (mm), Na-DOL (μm) is preferably (50×t-15) μm or more, more preferably (50×t+25) μm or more, even more preferably (50×t+45) μm or more, particularly preferably (50×t+65) μm or more, and most preferably (50×t+85) μm or more. On the other hand, from the viewpoint of suppressing the stress of the glass to a tensile stress below the CT limit, Na-DOL is preferably (100×t+95) μm or less, more preferably (100×t+90) μm or less, even more preferably (100×t+88) μm or less, particularly preferably (100×t+86) μm or less, and most preferably (100×t+84) μm or less.

[0132] From the viewpoint of increasing the drop strength, Na-CS0 (MPa) is preferably 150 MPa or more, more preferably 200 MPa or more, even more preferably 250 MPa or more, particularly preferably 280 MPa or more, and most preferably 300 MPa or more. On the other hand, from the viewpoint of suppressing the stress of the glass to a tensile stress equal to or less than the CT limit, Na-CS0 is preferably 650 MPa or less, more preferably 600 MPa or less, even more preferably 580 MPa or less, particularly preferably 550 MPa or less, and most preferably 520 MPa or less.

[0133] From the viewpoint of increasing bending strength, the compressive stress value CS1 (MPa) at a depth of 1 μm from the glass surface is preferably 700 MPa or more, more preferably 750 MPa or more, even more preferably 800 MPa or more, particularly preferably 850 MPa or more, and most preferably 900 MPa or more.

[0134] The compressive stress value CS2 (MPa) at a depth of 2 μm from the glass surface is preferably 550 MPa or more, more preferably 600 MPa or more, even more preferably 650 MPa or more, particularly preferably 700 MPa or more, and most preferably 750 MPa or more, from the viewpoint of increasing bending strength.

[0135] Compressive stress value CS at a depth of 50 μm from the glass surface 50 From the viewpoint of enhancing drop strength, where t (mm) is the thickness of the glass, (MPa) is preferably (140×t) MPa or more, more preferably (140×t+20) MPa or more, even more preferably (140×t+30) MPa or more, particularly preferably (140×t+40) MPa or more, and most preferably (140×t+50) MPa or more.

[0136] Compressive stress value CS at a depth of 90 μm from the glass surface 90 From the viewpoint of enhancing drop strength, where t (mm) is the thickness of the glass, (MPa) is preferably (40×t) MPa or more, more preferably (40×t+5) MPa or more, even more preferably (40×t+10) MPa or more, particularly preferably (40×t+20) MPa or more, and most preferably (40×t+30) MPa or more.

[0137] CTave (MPa) is a value equivalent to the average value of tensile stress, as determined by the above-mentioned method. From the viewpoint of increasing drop strength, when the thickness of the glass is t (mm), CTave is preferably (-50 x t + 88) MPa or more, more preferably (-50 x t + 90) MPa or more, even more preferably (-50 x t + 91) MPa or more, and most preferably (-50 x t + 92) MPa or more. On the other hand, from the viewpoint of suppressing the stress of the glass to a tensile stress below the CT limit, CTave is preferably lower than the value of CTA determined by formula (1).

[0138]

number

[0139] t: Plate thickness (mm) K1c: Fracture toughness value (MPa m 1 / 2 ) The value obtained by subtracting the value of CTave from the CTA is preferably 1 MPa or more, more preferably 2 MPa or more, and most preferably 3 MPa or more.

[0140] ICT (Pa·m) represents the integral value of tensile stress. From the viewpoint of increasing drop strength, when the thickness of the glass is t (mm), ICT is preferably (32235×t+1000) Pa·m or more, more preferably (32235×t+2000) Pa·m or more, even more preferably 32235×t+3000) Pa·m or more, particularly preferably 32235×t+4000) Pa·m or more, and most preferably (32235×t+5000 Pa·m or more. On the other hand, From the viewpoint of keeping the tensile stress below the CT limit of the glass, ICT is preferably (32235×t+27000) Pa·m or less, preferably (32235×t+25000) Pa·m or less, more preferably (32235×t+23000) Pa·m or less, particularly preferably (32235×t+20000) Pa·m or less, and most preferably (32235×t+15000) Pa·m or less.

[0141] (Glass for chemical strengthening and chemically strengthened glass) The glass for chemical strengthening and the chemically strengthened glass according to the above embodiments will be described.

[0142] The shape of the glass for chemical strengthening or the chemically strengthened glass is not particularly limited, but is typically a plate shape, and may be flat or curved. In addition, it may have a portion with a different thickness.

[0143] When the glass for chemical strengthening or the chemically strengthened glass is in the form of a plate, its thickness (t) is preferably 3000 μm or less, more preferably 2000 μm or less, 1600 μm or less, 1500 μm or less, 1100 μm or less, 900 μm or less, 800 μm or less, and 700 μm or less in the following stepwise manner. In addition, the thickness (t) is preferably 300 μm or more, more preferably 400 μm or more, and even more preferably 500 μm or more in order to obtain sufficient strength by the chemical strengthening treatment.

[0144] The chemically strengthened glass according to the embodiment of the present invention is suitable for obtaining chemically strengthened glass having high electrical resistance by chemical strengthening treatment and capable of suppressing abnormal light emission. In addition, the chemically strengthened glass according to the embodiment of the present invention is particularly useful as a cover glass used in electronic devices such as mobile devices such as mobile phones and smartphones, since it has high electrical resistance and can suppress abnormal light emission. Furthermore, it is also useful for cover glass of electronic devices such as televisions, personal computers, and touch panels that are not intended to be portable, elevator walls, and walls (full-surface displays) of buildings such as houses and buildings. It is also useful as building materials such as window glass, table tops, interiors of automobiles and airplanes, and cover glasses thereof, and for housings having curved shapes. That is, the present invention relates to an electronic device equipped with the chemically strengthened glass according to the embodiment of the present invention or the chemically strengthened glass according to the embodiment of the present invention.

[0145] (Glass for chemical strengthening and method for producing chemically strengthened glass) The glass for chemical strengthening and the method for producing chemically strengthened glass according to the present embodiment will be described. For example, when producing a plate-shaped glass for chemical strengthening, the glass raw materials are appropriately mixed so as to obtain glass having the above-mentioned composition, and are heated and melted in a glass melting furnace. The glass is then homogenized by bubbling, stirring, adding a clarifier, etc., formed into a glass plate of a predetermined thickness, and slowly cooled to obtain glass for chemical strengthening. Alternatively, the glass for chemical strengthening may be formed into a plate shape by a method of forming the glass into a block shape, slowly cooling it, and then cutting it to obtain glass for chemical strengthening. When the glass for chemical strengthening is crystallized glass, a heat treatment process for crystallization may be further included.

[0146] Examples of methods for forming into a plate include the float method, the press method, the fusion method, and the down-draw method. In particular, when producing a large glass plate, the float method is preferred. In addition, continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.

[0147] Chemically strengthened glass is obtained by subjecting the glass for chemical strengthening to an ion exchange treatment. For example, as the method for producing the glass according to the above-mentioned third to sixth embodiments, it is preferable to produce chemically strengthened glass using the glass for chemical strengthening according to the first or second embodiment, or to produce chemically strengthened glass by carrying out chemical strengthening by a preferred chemical strengthening process described below, and it is more preferable to produce chemically strengthened glass by using the composition of the glass according to the first or second embodiment as the base composition and carrying out chemical strengthening by a preferred chemical strengthening process described below.

[0148] In this embodiment, it is preferable to perform a two-stage ion exchange treatment. However, this does not in any way preclude the chemically strengthened glass according to each of the above-mentioned embodiments from being obtained by performing a one-stage ion exchange treatment or three or more stages of ion exchange treatment. When the two-stage ion exchange treatment is performed, a first alkali metal ion in the glass for chemical strengthening is exchanged with a second alkali metal ion in the first molten salt composition in the first ion exchange treatment, and a second alkali metal ion in the glass for chemical strengthening is exchanged with a third alkali metal ion in the second molten salt composition in the second ion exchange treatment.

[0149] In this specification, the term "molten salt composition" refers to a composition containing a molten salt. Examples of the molten salt contained in the molten salt composition include nitrates, sulfates, carbonates, and chlorides. Examples of the nitrates include lithium nitrate, sodium nitrate, potassium nitrate, cesium nitrate, rubidium nitrate, and silver nitrate. Examples of the sulfates include lithium sulfate, sodium sulfate, potassium sulfate, cesium sulfate, rubidium sulfate, and silver sulfate. Examples of the chlorides include lithium chloride, sodium chloride, potassium chloride, cesium chloride, rubidium chloride, and silver chloride. These molten salts may be used alone or in combination.

[0150] The molten salt composition is preferably one that is based on a nitrate, and more preferably one that is mainly composed of sodium nitrate or potassium nitrate. Here, "mainly composed" means that the content of the molten salt composition is 80 mass% or more.

[0151] A method for producing chemically strengthened glass according to this embodiment includes, for example, a first ion exchange treatment in which glass for chemical strengthening is brought into contact with a first molten salt composition, and after the first ion exchange treatment, a second ion exchange treatment in which the glass for chemical strengthening is brought into contact with a second molten salt composition, wherein the second molten salt composition has a potassium nitrate (KNO3) content of 94 mass% or more and a lithium ion content of less than 300 mass ppm.

[0152] In the above production method, it is preferable that the temperature of the second molten salt composition in the second ion exchange treatment is 380° C. to 450° C., and the time for which the second molten salt composition is brought into contact with the glass for chemical strengthening is 60 minutes or longer.

[0153] In the above production method, the second molten salt composition preferably contains 0 to 5 mass % of sodium nitrate (NaNO3).

[0154] The method for producing chemically strengthened glass according to this embodiment may be, for example, a method for producing chemically strengthened glass that includes subjecting glass for chemical strengthening to an ion exchange treatment to obtain chemically strengthened glass, and that obtains chemically strengthened glass having a K-DOL of 4.2 μm or more and a surface resistivity of 11 [log Ω / sq] or more.

[0155] The method for producing chemically strengthened glass according to this embodiment may also be, for example, a method for producing chemically strengthened glass that includes subjecting glass for chemical strengthening to an ion exchange treatment to obtain chemically strengthened glass, and that obtains chemically strengthened glass having a K-CSarea of ​​4000 Pa m or more and a surface resistivity of 11 [log Ω / sq] or more.

[0156] The first ion exchange treatment and the second ion exchange treatment will be described in detail below.

[0157] <<First ion exchange treatment>> In one embodiment, in the first ion exchange treatment, it is preferable to bring the glass for chemical strengthening containing a first alkali metal ion into contact with a first molten salt composition containing a second alkali metal ion having an ionic radius larger than that of the first alkali metal ion to perform ion exchange. In this embodiment, the second alkali metal ion is introduced into the glass for chemical strengthening by the first ion exchange treatment.

[0158] The composition of the first molten salt composition used in the first ion exchange treatment is not particularly limited as long as it does not impair the effects of the present invention, but as one embodiment, it preferably contains a second alkali metal ion having an ionic radius larger than that of the first alkali metal ion contained in the glass for chemical strengthening. The first molten salt composition preferably further contains a third alkali metal ion having an ionic radius larger than that of the second alkali metal ion.

[0159] In one embodiment, when the first alkali metal ion is a lithium ion, the second alkali metal ion is preferably a sodium ion, and the third alkali metal ion is preferably a potassium ion.

[0160] Examples of the molten salt containing sodium ions used in the first ionic molten salt composition include sodium nitrate, sodium sulfate, and sodium chloride, and among these, sodium nitrate is preferable.

[0161] In one embodiment, when the first molten salt composition contains sodium nitrate, the content is preferably 20% by mass or more and 100% by mass or less. Here, the lower limit of the content is more preferably 25% by mass or more, and even more preferably 30% by mass or more. Moreover, the upper limit of the content is more preferably 80% by mass or less, and even more preferably 60% by mass or less.

[0162] Examples of the molten salt containing potassium ions used in the first molten salt composition include potassium nitrate, potassium sulfate, and potassium chloride, and among these, potassium nitrate is preferable.

[0163] In one embodiment, when the first molten salt composition contains potassium nitrate, the content is preferably 20% by mass or more and 80% by mass or less. Here, the lower limit of the content is more preferably 30% by mass or more, even more preferably 40% by mass or more, and most preferably 50% by mass or more. Moreover, the upper limit of the content is more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0164] In the first ion exchange treatment, it is preferable to contact the glass for chemical strengthening with the first molten salt composition at a temperature of 380°C or higher. When the temperature of the first molten salt composition is 380°C or higher, the ion exchange is likely to proceed. It is more preferably 400°C or higher, further preferably 410°C or higher, and particularly preferably 420°C or higher. In addition, the temperature of the first molten salt composition is usually 450°C or lower from the viewpoints of the risk of evaporation and the composition change of the molten salt composition.

[0165] In the first ion exchange treatment, the time for contacting the glass for chemical strengthening with the first molten salt composition is preferably 0.5 hours or more since the surface compressive stress increases. The contact time is more preferably 1 hour or more. If the contact time is too long, not only the productivity decreases but also the compressive stress may decrease due to the relaxation phenomenon. Therefore, the contact time is usually 8 hours or less.

[0166] The first ion exchange treatment may be a one-stage treatment, or may be a two or more stage treatment under two or more different conditions (multi-stage strengthening).

[0167] <<Second ion exchange treatment>> The second ion exchange treatment is a step of, after the first ion exchange treatment, bringing the glass for chemical strengthening into contact with a second molten salt composition having a component ratio different from that of the first molten salt composition to perform ion exchange.

[0168] In the present production method, in the second ion exchange treatment, the second molten salt composition preferably contains a third alkali metal ion having an ionic radius larger than that of the second alkali metal ion. In the second molten salt composition, the content of the first alkali metal ion is preferably relatively small.

[0169] In one embodiment, when the second alkali metal ion is a sodium ion, the third alkali metal ion is preferably a potassium ion, and the first alkali metal ion is preferably a lithium ion.

[0170] Examples of the molten salt containing potassium ions used in the second molten salt composition include potassium nitrate, potassium sulfate, and potassium chloride, and among these, potassium nitrate is preferable.

[0171] In one embodiment, when the second molten salt composition contains potassium nitrate (KNO3), the content is preferably 94 mass% or more. Here, the lower limit of the content is more preferably 96 mass% or more, and even more preferably 98 mass% or more. The upper limit of the content may be 100 mass%, but is preferably 99.5 mass% or less, more preferably 99 mass% or less. When the second molten salt composition contains potassium nitrate, a relatively high content of potassium nitrate makes it easier to obtain a high resistance effect due to the size of the alkali metal ions substituted in the chemically strengthened glass, which is suitable for obtaining the chemically strengthened glass according to this embodiment.

[0172] The second molten salt composition may contain at least one of lithium ions and sodium ions. Examples of molten salts containing lithium ions used in the second molten salt composition include lithium nitrate, lithium sulfate, and lithium chloride, and among these, lithium nitrate is preferred. Examples of compositions containing sodium ions used in the second molten salt composition include sodium nitrate, sodium sulfate, and sodium chloride, and among these, sodium nitrate is preferred.

[0173] In the second molten salt composition, the content of lithium ions is preferably less than 300 ppm by mass, more preferably 200 ppm by mass or less, 100 ppm by mass or less, 80 ppm by mass or less, and further preferably 60 ppm by mass or less, in that order. This makes it possible to prevent lithium ions from penetrating into the surface layer of the chemically strengthened glass, resulting in a relatively low resistance. The content of lithium ions may be 0 ppm by mass, but may be 40 ppm by mass or more from the viewpoint of mass productivity of the chemically strengthened glass. When the second molten salt composition contains lithium nitrate (LiNO3), it is preferable that the content of lithium ions in the second molten salt composition is in the above-mentioned preferred range.

[0174] When the second molten salt composition contains sodium nitrate (NaNO3), the content is preferably 0.5 mass% or more, more preferably 1 mass% or more, and even more preferably 1.5 mass% or more. From the viewpoint of maintaining a high surface layer stress, the content is preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less.

[0175] In the second ion exchange treatment, it is preferable to bring the glass for chemical strengthening into contact with the second molten salt composition at 450°C or less. When the temperature of the second molten salt composition is 450°C or less, changes in the molten salt composition can be suppressed. The temperature of the second molten salt composition is more preferably 440°C or less, further preferably 430°C or less, and particularly preferably 420°C or less. In addition, from the viewpoint of accelerating the ion exchange, the temperature of the second molten salt composition is preferably 380°C or more, more preferably 390°C or more, and further preferably 400°C or more.

[0176] In the second ion exchange treatment, the time (treatment time) for contacting the glass for chemical strengthening with the second molten salt composition is preferably 60 minutes or more, more preferably 90 minutes or more, and even more preferably 120 minutes or more, from the viewpoint of stable ion exchange. On the other hand, the contact time in the second ion exchange treatment is preferably 300 minutes or less, more preferably 240 minutes or less, and even more preferably 180 minutes or less, from the viewpoint of lowering productivity if the contact time is too long. EXAMPLES

[0177] The present invention will be described below with reference to examples, but the present invention is not limited thereto. <Preparation of amorphous glass and glass-ceramic> The glass raw materials were mixed to obtain the following composition expressed in mole percentage based on oxides, and weighed out to make 400 g of glass. The mixed raw materials were then placed in a platinum crucible and placed in an electric furnace at 1500-1700°C, melted for about 3 hours, degassed, and homogenized. The K1c of glass material A was 0.8 (MPa m 1 / 2 ) was. Glass material A: SiO2 66%, Al2O3 11%, Y2O3 0.5%, ZrO2 1.3%, Li2O 11%, Na2O 5.5%, K2O 1.5%, MgO 3%, other components 0.3%. The ratio of the total content of Li2O, Na2O and K2O to the content of Al2O3 in glass material A (R2O / Al2O3) is 1.6. Glass material B: SiO2 65%, Al2O3 16%, P2O 51.2%, Li2O 7.5%, Na2O 5%, K2O 0.5%, MgO 0.5%, CaO 1.3%, B2O3 3%. The ratio of the total content of Li2O, Na2O and K2O to the content of Al2O3 in glass material B (R2O / Al2O3) is 0.8. Glass material C: SiO2 70%, Al2O3 11.5%, P2O 50.3%, Li2O 9%, Na2O 2.5%, K2O 0.2%, MgO 0.8%, CaO 2.6%, ZrO2 0.1%, B2O3 3%. The ratio of the total content of Li2O, Na2O and K2O to the content of Al2O3 in glass material C (R2O / Al2O3) is 1.0.

[0178] The obtained molten glass was poured into a metal mold, held at a temperature about 50°C higher than the glass transition point for 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block. The obtained molten glass was poured into a mold, held at a temperature near the glass transition point (714°C) for about 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block.

[0179] The obtained glass block was cut, ground, and finally mirror-polished on both sides to obtain a glass plate (glass for chemical strengthening) having a size of 120 mm x 60 mm and a thickness of 0.70 mm.

[0180] <Evaluation of chemical strengthening treatment and chemically strengthened glass> The glass plate obtained above was immersed in a molten salt composition under the conditions shown in Tables 1 and 2 to perform a first ion exchange treatment and a second ion exchange treatment, thereby obtaining chemically strengthened glass of Examples 1 to 16. Examples 1, 2, 5, 6, 13 to 15, 17, and 18 are working examples, and Examples 3, 4, 7 to 12, and 16 are comparative examples. The obtained chemically strengthened glass was evaluated by the following method.

[0181] [Stress measurement using a scattered light photoelastic stress meter] The stress of the chemically strengthened glass was measured by the method described in International Publication No. 2018 / 056121 using a scattered light photoelastic stress meter (SLP-2000 manufactured by Orihara Seisakusho). In addition, the stress profile was calculated using the attached software [SlpV (Ver. 2019.11.07.001)] of the scattered light photoelastic stress meter (SLP-2000 manufactured by Orihara Seisakusho).

[0182] The function used to obtain the stress profile is σ(x) = [a1 × erfc(a2 × x) + a3 × erfc(a4 × x) + a5]. i ( i = 1 to 5) are fitting parameters, and erfc is the complementary error function. The complementary error function is defined by the following equation.

[0183]

number

[0184] In the evaluation in this specification, the fitting parameters were optimized by minimizing the residual sum of squares between the obtained raw data and the above function. The measurement processing conditions were single shot, and the measurement area processing adjustment items were selected as follows: edge method on the surface, 6.0 μm for the inner surface end, automatic for the inner left and right ends, automatic (center of the sample thickness) for the inner deep end, and the extension of the phase curve to the center of the sample thickness was selected as a fitting curve.

[0185] The stress in the glass surface layer within a distance of several tens of μm from the glass surface was measured using a glass surface stress meter (FSM6000-UV manufactured by Orihara Seisakusho) according to the methods described in WO 2018 / 056121 and WO 2017 / 115811.

[0186] At the same time, the concentration distribution of alkali metal ions (sodium ions, potassium ions, and lithium ions) in the cross-sectional direction was measured using an EPMA (Electron Probe Micro Analyzer) and it was confirmed that there was no inconsistency with the obtained stress profile.

[0187] In addition, from the above measurement results and the obtained stress profile, K-CS0, K-DOL, K-CSarea, Na-CS0, Na-DOL, Na-CSarea, CS1, CS2, CS 50 , C.S. 90 The values ​​of CTmax, CTave, and ICT were obtained, and the results are shown in Tables 1 and 2.

[0188] <Measurement of resistivity> For each of the chemically strengthened glasses, the surface resistivity and the volume resistivity were measured by the following method. (Preparation of glass samples and film formation process) The glass sample used was 120mm x 60mm x 0.7mm. Prior to measuring the surface resistivity, a film was formed using the following procedure. A sputtering device was used to form a film on the 120 x 60 x 0.7mm glass sample. A platinum target was used as the film formation target, and argon was introduced to form a 30nm platinum film on the glass surface. When forming the film, a 60mm square pattern was performed based on JIS R3256:1998. (Surface resistivity) The surface resistivity was measured by the following method. The measurement device used was an ultra-microcurrent meter. The surface resistivity was measured by a three-terminal method in accordance with JIS C2141:1992 and JIS R3256:1998. The applied voltage was 100 V, and the value was measured 180 seconds after the voltage application. The discharge time was 3 seconds. (Volume Resistivity) The volume resistivity was measured by the following method. The measurement device used was an ultra-microcurrent meter. The glass sample used was 120×60×0.7 mm. The measurements were performed according to JIS C2141:1992 and JIS R3256:1998 using the three-terminal method. The applied voltage was 100 V, and the value 180 seconds after the voltage application was measured. The discharge time was 3 seconds.

[0189] The results are shown in Tables 1 and 2. Figure 2 is a diagram showing the relationship between the surface resistivity and the volume resistivity for the chemically strengthened glass of each example. Figure 3 is a diagram showing the relationship between the measured value of the volume resistivity and the value of Y for the chemically strengthened glass of each example. The value of Y is defined by the following formula. Y = -0.5984x1 + 0.00018x2 + 4.319×10 -7 x3 + 8.5 x1: Concentration of LiNO3 (mass%) in the molten salt used for the final ion exchange treatment during the chemical strengthening treatment x2: Product of K-CS0 and K-DOL, K-CSarea (Pa·m) x3: Product of Na-CS0 and Na-DOL, Na-CSarea (Pa·m)

[0190] <K2O concentration, Li2O concentration> The K2O concentration at a depth x (μm) and the Li2O concentration at a depth x (μm) were measured by the above method. From these results, K2O@3μm, K2O@center, Li2O@5μm, and Li2O@center were obtained. The results are shown in Tables 1 and 2. In addition, Figure 4 shows the K2O profiles of the surface layers of Examples 1, 2, 4, and 5. As shown in Figure 4, the concentration of potassium ions in the surface layer of 3 μm varies for each sample, and as shown in Tables 1 and 2, it can be confirmed that there is a correlation between the surface resistivity and the volume resistivity of potassium ions in the surface layer of 3 μm.

[0191] Explanations of each notation in Tables 1 and 2 are shown below. K-CS0: Compressive stress value (MPa) caused by potassium ions at a depth of 0 μm measured by FSM K-DOL: Value of the depth from the glass surface of the compressive stress layer caused by potassium ions (μm) K-CS area: CS0 × K-DOL (Pa·m) Na-CS0: Compressive stress value (MPa) caused by Na ions at a depth of 0 μm measured by SLP Na-DOL: Depth from the glass surface of the compressive stress layer caused by sodium ions (μm) Na-CS area:Na-CS0×Na-DOL(Pa m) CS x : Compressive stress value at depth of x μm (MPa) CTave=ICT / L CT (MPa) ICT: Integrated value of tensile stress (Pa m) L CT : Length of tensile stress region in the thickness direction (μm) CTmax: Maximum tensile stress K2O@3μm: K2O concentration at a depth of 3μm from the surface (mol%) KO@center: KO concentration at the center of the plate thickness (mol%) Li2O@3μm: Li2O concentration at a depth of 3μm from the surface (mol%) Li2O@center: Li2O concentration at the center of the plate thickness (mol%)

[0192] [Table 1]

[0193] [Table 2]

[0194] As shown in Tables 1 and 2, Examples 1, 2, 5, 6, 13 to 15, 17, and 18, which had a K-DOL of 4.2 μm or more, had a large surface resistivity of 11 [log Ω / sq] or more compared to the comparative example.

[0195] Examples 1, 2, 5, 6, 13 to 15, 17, and 18, in which the K-CSarea was 4000 Pa·m or more, had a large surface resistivity of 11 [log Ω / sq] or more compared to the comparative example.

[0196] Examples 1, 2, 5, 17, and 18, in which the ratio of the K2O concentration at a depth of 3 μm from the glass surface (K2O@3μm) to the K2O concentration at the center of the sheet thickness (K2O@center) was 5.5 or more, had a higher surface resistivity than the comparative examples, being 11 [logΩ / sq] or more.

[0197] Examples 1, 5, 17, and 18, in which the ratio of the Li2O concentration at a depth of 5 μm from the glass surface (Li2O@5μm) to the Li2O concentration at the center of the plate thickness (Li2O@center) was 0.85 or less, had a higher surface resistivity than the comparative example, being 11 [logΩ / sq] or more. [Explanation of symbols]

[0198] 10 OLED Display 11 Coverslip 12 Charge 13 OLED light emitting device 14 Polyimide substrate 15 Cathode 16 TFT array< / ctave>

Claims

1. In terms of mole percentage based on oxide, SiO 2 More than 50% B 2 O 3 0 to 10% Al 2 O 3 を1~30%、 P 2 O 5 0 to 10%, Y 2 O 3 を0~10%、 Li 2 Oを0~25%、 Na 2 Oを0~25%、 K 2 O 0 to 25%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 10%, BaO 0 to 10%, ZnO 0-10%, ZrO 2 0 to 5%, TiO 2 0 to 5%, SnO 2 0 to 5%, Fe 2 O 3 Contains 0 to 0.5% A 2 O 3 Li relative to the content 2 O, Na 2 O and K 2 The ratio of the total content of O (R 2 O / Al 2 O 3 ) satisfies the following formula (A): (A) 0.8≦(R) 2 O / Al 2 O 3 )≦30

2. In terms of mole percentage based on oxide, Li 2 Oを7~12%、 Na 2 Oを1.5~6%、 K 2 The glass for chemical strengthening according to claim 1, containing 0 to 1.5% O.

3. The K-DOL defined below is 4.2 μm or more, and Chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more. K-DOL (μm): Depth from the glass surface of the compressive stress layer caused by potassium ions

4. The K-CS area defined below is 4000 Pa m or more, and Chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more. K-CSarea (Pa・m):K-CS 0 and the product of K-DOL K-CS 0 (MPa): compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): Depth from the glass surface of the compressive stress layer caused by potassium ions

5. Said K-CS 0 The chemically strengthened glass according to claim 4, wherein the compressive strength is 800 MPa or more.

6. K at a depth of 3 μm from the glass surface 2 O concentration, K 2 K at the center of thickness of 3 μm 2 O concentration, K 2 The ratio of O@center is 5.3 or more, Chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more.

7. Li at a depth of 5 μm from the glass surface 2 O concentration Li 2 O @ 5 μm, Li at the center of the plate thickness 2 O concentration Li 2 The ratio to O@center is 0.85 or less, Chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more.

8. The chemically strengthened glass according to claim 3, wherein the value of Y defined below is 9.4 or more. Y=0.00018x 1 +4.319×10 -7 x 2 +8.5 x 1 : K-CS 0 and the product of K-DOL, K-CSarea (P a m) x 2 : Na-CS 0 and the product of Na-DOL Na-CSarea (Pa m) K-CS 0 (MPa): compressive stress value on the glass surface measured by a glass surface stress meter K-DOL (μm): Depth from the glass surface of the compressive stress layer caused by potassium ions Na-CS 0 (MPa): compressive stress value on the glass surface measured with a scattered light photoelastic stress meter Na-DOL (μm): Depth from the glass surface of the compressive stress layer caused by Na ions

9. An electronic device comprising the chemically strengthened glass according to claim 1 or 2 or the chemically strengthened glass according to any one of claims 3 to 8.

10. A first ion exchange treatment in which the glass for chemical strengthening is brought into contact with a first molten salt composition; A method for producing chemically strengthened glass, comprising: a second ion exchange treatment in which the glass for chemical strengthening is contacted with a second molten salt composition after the first ion exchange treatment; The second molten salt composition is KNO 3 The content of is 94% by mass or more and the content of lithium ions is less than 300 ppm by mass.

11. 11. The method for producing chemically strengthened glass according to claim 10, wherein the temperature of the second molten salt composition in the second ion exchange treatment is 380 ° C. to 450 ° C., and the time for which the second molten salt composition is contacted with the glass for chemical strengthening is 60 minutes or longer.

12. The second molten salt composition is NaNO 3 The method for producing chemically strengthened glass according to claim 10 or 11, comprising 0 to 5 mass%.

13. A method for producing chemically strengthened glass, comprising subjecting chemically strengthened glass to an ion exchange treatment, The K-DOL defined below is 4.2 μm or more, and A method for producing chemically strengthened glass, which obtains chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more. K-DOL (μm): Depth from the glass surface of the compressive stress layer caused by potassium ions

14. A method for producing chemically strengthened glass, comprising subjecting chemically strengthened glass to an ion exchange treatment, The K-CS area defined below is 4000 Pa m or more, and A method for producing chemically strengthened glass, which obtains chemically strengthened glass having a surface resistivity of 11 [log Ω / sq] or more. K-CSarea (Pa・m):CS 0 and the product of K-DOL C.S. 0 (MPa): compressive stress value on the glass surface K-DOL (μm): Depth from the glass surface of the compressive stress layer caused by potassium ions

Citation Information

Patent Citations

  • Glass, chemically strengthened glass, and cover glass

    WO2021010376A1