Sintered body and its manufacturing method, dental prosthetic material, and denture for anterior teeth
A zirconia-based powder composition with varied stabilizing elements optimizes sintering behavior for short-time processing, addressing the need for high strength and translucency in dental prosthetics, particularly anterior dentures, while minimizing sintering duration.
Patent Information
- Application Number
- JP2024143405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-16
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-15
AI Technical Summary
Existing sintered zirconia-based dental prosthetics face challenges in achieving both high mechanical strength and translucency, particularly for anterior teeth, while also requiring long sintering times that increase patient burden.
A powder composition and calcined body with zirconia as a matrix, containing two or more stabilized zirconias with different stabilizing element contents, optimized for short-time sintering, which controls sintering behavior by adjusting surface activity and particle interface states to achieve desired optical and mechanical properties.
The solution results in a sintered body with sufficient translucency and mechanical strength for dental prosthetics, especially anterior dentures, while reducing sintering time, thus enhancing patient convenience.
Smart Images

Figure 2024161088000007 
Figure 2024161088000008 
Figure 2024161088000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a powder composition containing zirconia as a main component, a calcined body, a sintered body, and methods for producing the same. [Background technology]
[0002] Sintered bodies with a zirconia matrix (base material) that are used for dental prosthetic materials such as crowns and bridges are required to have the same aesthetic quality as natural teeth. To meet this requirement, studies have been conducted to improve the translucency of sintered bodies by increasing the content of stabilizing elements (Patent Document 1).
[0003] However, the mechanical strength of a sintered body with a zirconia matrix decreases significantly with an increase in the content of the stabilizing element. In response to this, a sintered body that satisfies the high mechanical strength required for dental prosthetic materials has been disclosed (Patent Document 2), despite the content of the stabilizing element being considered to cause a decrease in mechanical strength when crystal particles with different contents of the stabilizing element are included in the sintered body (Patent Document 2).
[0004] On the other hand, the sintered bodies described in Patent Documents 1 and 2 are produced by sintering that requires a holding time at the maximum temperature of 2 hours and 7 hours or more for heating, holding, and cooling (hereinafter also referred to as "normal sintering"). Therefore, a long sintering time was required to produce these sintered bodies.
[0005] In recent years, dental treatment using sintered bodies produced by applying a sintering method that requires a shorter sintering time than normal sintering, so-called short-time sintering, has been considered. Chairside treatment is expected to reduce the burden on patients who have to visit the hospital.
[0006] Patent Document 3 discloses a sintered body obtained by short-time sintering, which has a matrix of zirconia containing 4 mol% to 6 mol% of a stabilizing element and contains undissolved yttria. Patent Document 4 discloses a sintered body obtained by short-time sintering, which has a matrix of 4 mol% to 5.5 mol% of zirconia and has a contrast ratio of 0.68 to 0.70. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2015-143178 [Patent Document 2] Japanese Patent Application Publication No. 2021-059489 [Patent Document 3] International Publication No. 2018 / 056330 [Patent Document 4] Japanese Patent Application Publication No. 2020-033338 Summary of the Invention [Problem to be solved by the invention]
[0008] The sintered body of Patent Document 3 does not have sufficient mechanical strength because it contains undissolved yttria. In Patent Document 4, even if a sintered body with a high yttria content is produced by short-time sintering, the obtained sintered body does not have translucency applicable to a front tooth denture, and furthermore, the translucency is about the same as that of a sintered body with an yttria content of 4 mol% obtained by normal sintering. The present disclosure aims to provide at least one of a powder composition and a calcined body, which have a matrix of zirconia with a high content of stabilizing elements and can be sintered in a short time to obtain a sintered body that satisfies the translucency and mechanical strength required for a dental prosthesis, particularly a front tooth denture, and a method for producing the same. [Means for solving the problem]
[0009] The present inventors have studied the sintering of powders and calcined bodies having a matrix of zirconia with a high content of stabilizing elements. As a result, they have found that it is difficult to obtain sintered bodies having the same translucency as sintered bodies obtained by normal sintering, and furthermore, sintered bodies having properties suitable for use as an anterior denture, even if short-time sintering is simply applied to powders and calcined bodies having a matrix of zirconia with a high content of stabilizing elements. Furthermore, the present inventors have found that the sintering behavior in the first half of the sintering period has a large effect on densification in short-time sintering.
[0010] Based on these findings, the inventors focused on the surface activity of each particle constituting the powder and the calcined body, and came up with the idea of making particles with different surface activities coexist in a specific relationship to change the state of the interface between the particles. It was then discovered that this would allow the sintering behavior in the first half of the sintering process to be controlled. As a result, the inventors have completed the powder composition and calcined body of the present disclosure, which have a matrix of zirconia with a high content of stabilizing elements and which can produce a sintered body that satisfies the translucency required for dental prosthetic materials, particularly anterior dentures, even when a sintering method that can be applied to chairside treatment is applied.
[0011] That is, the present invention is as defined in the claims, and the gist of the present disclosure is as follows. [1] Contains two or more stabilized zirconias with different contents of stabilizing elements, the content of the stabilizing elements is more than 4.0 mol% and not more than 5.8 mol%, and the rate of change of the thermal shrinkage rate per unit temperature at 1300°C is 0.07%°C ―1 and further comprising a content of a stabilizing element in the stabilized zirconia of 8.0 mol % or less. [2] The powder composition according to [1] above, wherein the stabilized zirconia comprises a first stabilized zirconia having a stabilizing element content of 1.0 mol% or more and 5.0 mol% or less, and a second stabilized zirconia having a stabilizing element content of 3.0 mol% or more and 8.0 mol% or less. [3] The rate of change in thermal contraction per unit temperature at 1500°C is 0.02%°C. ―1The powder composition according to the above [1] or [2]. [4] The powder composition according to any one of [1] to [3] above, wherein the stabilizing element is one or more selected from the group consisting of yttrium, calcium and magnesium. [5] BET specific surface area is 8m 2 / g or more 13m 2 The powder composition according to any one of [1] to [4] above, wherein the molecular weight is 1000 or less. [6] The powder composition according to any one of [1] to [5] above, wherein the proportion of tetragonal and cubic crystals in the crystal phase is 65% or more. [7] Contains two or more stabilized zirconias with different stabilizing element contents, the stabilizing element content is more than 4.0 mol% and not more than 5.8 mol%, and the rate of change of thermal shrinkage per unit temperature at 1300°C is 0.07%°C ―1 and further comprising a content of a stabilizing element in the stabilized zirconia of 8.0 mol % or less. [8] The calcined body according to the above item [7], wherein the stabilized zirconia comprises a first stabilized zirconia having a stabilizing element content of 1.0 mol% or more and 5.0 mol% or less, and a second stabilized zirconia having a stabilizing element content of 3.0 mol% or more and 8.0 mol% or less. [9] The rate of change of thermal contraction per unit temperature at 1500°C is 0.02%°C. ―1 The calcined body according to the above [7] or [8].
[10] The calcined body according to any one of the above [7] to [9], wherein the stabilizing element is one or more selected from the group consisting of yttrium, calcium and magnesium.
[11] The calcined body according to any one of [7] to
[10] above, wherein the proportion of tetragonal and cubic crystals in the crystal phase is 75% or more.
[12] A method for producing a sintered body, comprising using a powder composition according to any one of [1] to [6] or a calcined body according to any one of [7] to
[11] above.
[13] A sintered body obtained by sintering the powder composition according to any one of [1] to [6] above.
[14] A sintered body obtained by sintering the calcined body according to any one of [7] to
[11] above.
[15] A sintered body having a matrix of zirconia containing a stabilizing element, the content of the stabilizing element being more than 4.0 mol% and not more than 5.8 mol%, an average crystal grain size being not more than 2.5 μm, a crystal grain size difference being not more than 0.10 μm, and a tetragonal prime phase ratio being not less than 70%. Effect of the Invention
[0012] The present disclosure achieves the objective of providing at least one of a powder composition and a calcined body, which have a matrix of zirconia with a high content of stabilizing elements and which can be sintered in a short period of time to obtain a sintered body that satisfies the translucency required for dental prosthetic materials, particularly dentures for anterior teeth, and a method for producing the same. [Brief description of the drawings]
[0013] [Figure 1] This is an example of a TEM observation image used in STEM-EDS measurement. [Diagram 2] This is an example of a TEM observation image used in STEM-EDS measurement. [Diagram 3] 4 is a graph showing the frequency distribution of the amount of stabilizing elements in the powder composition obtained in Example 2. [Figure 4] 1 is a graph showing the frequency distribution of the amounts of stabilizing elements in the calcined bodies obtained in Example 11. [Diagram 5] 13 is a graph showing the frequency distribution of the amounts of stabilizing elements in the calcined body obtained in Comparative Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The powder composition of the present disclosure will be described with reference to an embodiment. The definitions of terms used in the embodiment are as follows.
[0015] The term "composition" refers to a substance having a certain composition, and includes, for example, one or more selected from the group consisting of powder, granules, molded body, calcined body, and sintered body. The term "zirconia composition" refers to a composition essentially consisting of zirconia, and further, a composition having zirconia as a matrix (base material).
[0016] A "powder" is a composition that is an aggregate of powder particles (powder-like particles) and has flowability. A "zirconia powder" is a powder that is essentially made of zirconia, or a powder that has zirconia as a matrix (base material). A "powder composition" is a composition that is composed of powders with different characteristics, and in particular, a composition that contains powders with different compositions.
[0017] The term "granular powder" refers to a composition that is an aggregate of powder particles and has flowability, particularly a composition in which the powder particles are in a slow aggregate state. The term "zirconia granular powder" refers to a granular powder that is essentially made of zirconia, and further, a granular powder that has zirconia as a matrix (base material).
[0018] A "molded body" is a composition having a certain shape composed of powder particles aggregated by physical force, and in particular, a composition in a state in which no heat treatment has been performed after the shape has been imparted (e.g., after molding). A "zirconia molded body" is a molded body essentially made of zirconia, and further, a molded body having zirconia as a matrix (parent material). The term "molded body" is also used interchangeably with "powder compact."
[0019] The term "calcined body" refers to a composition having a certain shape composed of fused particles, which is heat-treated at a temperature below the sintering temperature. The term "zirconia calcined body" refers to a calcined body essentially made of zirconia, and further refers to a calcined body having zirconia as a matrix (base material).
[0020] A "sintered body" is a composition having a certain shape composed of crystal grains, and is a composition in a state in which it has been heat-treated at a temperature equal to or higher than the sintering temperature. A "zirconia sintered body" is a sintered body essentially made of zirconia, and further, a sintered body having zirconia as a matrix (base material).
[0021] The term "stabilizing element" refers to an element that has the function of stabilizing the crystal phase of zirconia by dissolving in the zirconia.
[0022] The content (mol %; hereinafter also referred to as "amount of stabilizing element") of a composition (e.g., powder composition, calcined body, sintered body) of a stabilizing element is the molar ratio of the stabilizing element converted into an oxide to the total of zirconium converted into ZrO2 and the stabilizing element converted into an oxide in the composition. For example, when only yttrium is contained as a stabilizing element, the amount of the stabilizing element (amount of yttrium) is the molar ratio of yttria (Y2O3) to the total of zirconium converted into ZrO2 and yttrium converted into an oxide (i.e., yttria: Y2O3) in the composition.
[0023] The "amount of change in heat shrinkage per unit temperature (hereinafter also referred to as the "rate of change in heat shrinkage" or "ΔV")" is a physical property inherent to a composition, and is the amount of change in the heat shrinkage of the composition per unit temperature at a specific temperature. The rate of change in heat shrinkage in this embodiment is calculated by the following formula.
[0024] ΔV = ΔL / ΔT = {|L(T2)-L(T1)|} / (T2-T1) In the above formula, ΔV is the rate of change of the thermal shrinkage rate [%℃ -1 ], ΔT is the difference between temperatures T1 and T2 [℃], where T2-T1=3±0.5 [℃]. ΔL is the difference [%] between the thermal shrinkage rate at temperature T1 (L(T1)) and the thermal shrinkage rate at temperature T2 (L(T2)).
[0025] The thermal shrinkage rate L(T) [%] at temperature T is calculated from the measurement results of the amount of thermal shrinkage (l-l0) during the temperature rise process using formula (1).
[0026]
number
[0027] In formula (1), L(T) is the thermal shrinkage rate [%] at temperature T, l is the length [mm] of the molded body at temperature T, l0 is the length [mm] of the molded body before heat treatment, T is the measurement temperature [°C], T0 is the temperature at the start of measurement [°C], and β is a coefficient (11.1 × 10 -6 ℃ -1 ).
[0028] The amount of thermal shrinkage can be obtained by measuring the amount of thermal shrinkage using a general thermal dilatometer (for example, TD5000SE, manufactured by NETZSCH). The conditions for measuring the amount of thermal shrinkage include the following.
[0029] Atmosphere: Air flow (100mL / min) Heating rate: 20℃ / min Maximum temperature reached: 1600℃ Measurement sample: Molded body Diameter 6mm Length: 15±2mm Shape: Cylindrical Standard sample: Alumina Diameter 6mm Length (length of measurement sample)-(1.5±0.5)mm Shape: Cylindrical
[0030] The molded body used as the measurement sample may be a molded body obtained by filling a powder sample into a mold, uniaxially molding at a pressure of 19.6 MPa, and then CIP processing at a pressure of 196 MPa, or a calcined body obtained by calcining the molded body. In addition, when the molded body contains a molding aid, the measurement sample (molded body) may be heat-treated in air at 700°C for 1 hour prior to the measurement.
[0031] When measuring the amount of thermal shrinkage, the sample is heated with a load of 0.01 kg applied in the length direction of the sample. After the temperature rise starts, the temperature T and the length (l) of the sample at that temperature are measured every 3 seconds, and L(T) is calculated from the above formula (1). ΔL is derived from L(T) at two temperatures T1 and T2 that satisfy the relationship ΔT=3±0.5°C.
[0032] The thermal contraction amount is measured by using alumina as a standard sample, and the thermal expansion of the standard sample is corrected using general thermal analysis software (for example, TD5000SE analysis software Ver. 5.0.2, manufactured by NETZSCH).
[0033] The "BET specific surface area" may be measured by a BET multipoint method (5 points) using nitrogen as the adsorption gas in accordance with JIS R 1626. Specific measurement conditions for the BET specific surface area include the following conditions.
[0034] Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing in air at 250℃ for 1 hour or more
[0035] The BET specific surface area can be measured using a common device (for example, Tristar II 320, manufactured by Shimadzu Corporation).
[0036] The "tetragonal and cubic crystal ratio (hereinafter also referred to as "T+C phase ratio")" is the total ratio of tetragonal and cubic crystals in the crystal phase, and is a value calculated from the powder X-ray diffraction (hereinafter also referred to as "XRD") pattern of the composition using formula (2).
[0037] f T+C =[I t (111)+I c (111)] / [I m (111)+I m (11-1)+I t (111)+I c (111)] (2) In formula (2), f T+C is the tetragonal and cubic crystal ratio, It (111) is the surface intensity of the tetragonal (111) plane, I c (111) is the surface intensity of the cubic (111) plane, I m (111) is the surface intensity of the monoclinic (111) plane, I m (11-1) is the area intensity of the monoclinic (11-1) plane.
[0038] The area intensity of each crystal plane can be obtained by profile fitting the XRD pattern after smoothing and background removal processing using a divided pseudo-Voigt function. Smoothing processing, background processing, and analysis of the XRD pattern such as calculation of area intensity can be performed using an analysis program attached to the X-ray diffractometer (e.g., Integrated Powder X-ray Analysis Software PDXL Ver.2.2, manufactured by RIGAKU Corporation).
[0039] The XRD pattern in this embodiment is preferably obtained by XRD measurement under the following conditions. Radiation source: CuKα radiation (λ=0.15418nm) Measurement mode: Continuous scan Scan speed: 2° / min Measurement range: 2θ=26°~33° 2θ=72°~76° Acceleration voltage / current: 40mA / 40kV Divergence vertical limit slit: 10mm Divergence / entrance slit: 1° Receiving slit: open Detector: Semiconductor detector (D / teX Ultra) Filter: Ni filter Goniometer radius: 185mm
[0040] XRD measurement can be performed using a general X-ray diffractometer (e.g., Ultima IV, manufactured by RIGAKU). If the composition is a calcined body, its surface is polished with sandpaper of grain size #400 according to JIS R 6001-2, and then the surface is lapped with a diamond abrasive of grain size 3 μm, and XRD measurement can be performed on the surface. If the composition is a sintered body, its surface is polished to a surface roughness Ra≦0.02 μm, and XRD measurement can be performed on the surface.
[0041] Examples of XRD peaks corresponding to each crystal plane of zirconia measured in the above-mentioned XRD measurement include XRD peaks having peak tops at the following 2θ. XRD peak corresponding to monoclinic (111) plane: 2θ=31±0.5° XRD peak corresponding to monoclinic (11-1) plane: 2θ=28±0.5° XRD peak corresponding to tetragonal (111) plane: 2θ=30±0.5° XRD peak corresponding to cubic (111) plane: 2θ=30±0.5°
[0042] The XRD peak corresponding to the tetragonal (111) plane and the XRD peak corresponding to the cubic (111) plane are measured as a single overlapping peak. Therefore, I t (111)+I c (111) can be determined from the integrated intensity of one XRD peak having a peak top at 2θ=30±0.5°.
[0043] The "tetragonal prime phase ratio (hereinafter also referred to as the "T' phase ratio")" is the ratio of the tetragonal prime phase to the crystal phase, and the "cubic crystal ratio (hereinafter also referred to as the "C phase ratio")" is the ratio of the cubic crystal to the crystal phase. These values are calculated from the XRD pattern of the surface of the sintered body using formulas (3) and (4).
[0044] f T’ =[I t’ (004)+I t’ (400)] / [It (004)+I t (400)+I t’ (004)+I t’ (400)+I c (400)] (3) f c =[I c (400)] / [I t (004)+I t (400)+I t’ (004)+I t’ (400)+I c (400)] (4) In formula (3) and formula (4), f T’ is the T' phase ratio, f C is the C phase ratio, I t’ (004) is the surface intensity of the tetragonal prime (004) plane, I t’ (400) is the area intensity of the tetragonal prime (400) plane, I t (004) is the surface intensity of the tetragonal (004) plane, I t (400) is the surface intensity of the tetragonal (400) plane, and I c (400) is the area intensity of the cubic (400) plane.
[0045] The XRD pattern and the area intensity of each crystal plane may be determined in a manner similar to that described in relation to formula (2).
[0046] Examples of XRD peaks corresponding to each crystal plane measured in the above-mentioned XRD measurement include XRD peaks having peak tops at the following 2θ. XRD peak corresponding to tetragonal (004) plane: 2θ=72.9±0.1° XRD peak corresponding to tetragonal prime (004) plane: 2θ=73.3±0.1° XRD peak corresponding to tetragonal prime (400) plane: 2θ=73.9±0.1° XRD peak corresponding to tetragonal (400) plane: 2θ=74.3±0.1° XRD peak corresponding to cubic (400) plane: 2θ=73.7±0.05°
[0047] The "average particle size" is D50 in the volume particle size distribution of a powder or powder composition measured by a wet method, and can be measured using a general device (e.g., MT3300EXII, manufactured by Microtrack Bell). As a measurement sample, a powder from which slow aggregation has been removed by a dispersion treatment such as ultrasonic treatment is dispersed in pure water to form a slurry. The measurement of the volume particle size distribution by the wet method is preferably performed by setting the pH of the slurry to 3.0 to 6.0.
[0048] The "average granule particle size" is D50 in the volumetric particle size distribution of granular powder measured by the dry method, and can be measured using a general device (e.g., MT3100II, manufactured by Microtrack Bell). The measurement sample is the granular powder in a slowly agglomerated state, without undergoing any dispersion treatment such as ultrasonic treatment.
[0049] The "average crystal grain size" is the average diameter based on the number of crystal grains constituting the sintered body, and is obtained by observing a region of the sintered body from the surface to 1% of the surface in the thickness direction of the sintered body with a scanning electron microscope (hereinafter also referred to as "SEM") and analyzing the image of the SEM observation image. That is, the cross section of the sintered body is used as an observation sample, and any region from the surface of the sintered body to 1% of the surface in the thickness direction of the sintered body is observed with an SEM to obtain the SEM observation image.
[0050] SEM observation may be performed using a general scanning electron microscope (e.g., JSM-IT500LA, manufactured by JEOL Ltd.). SEM observation may be performed by appropriately setting the observation magnification so that the number of crystal particles to be image-analyzed (crystal particles in which the crystal grain boundaries are observed without interruption in the SEM observation image (described later)) is 450±50. In order to suppress variation in the observed crystal particles due to differences in the SEM observation locations, it is preferable to obtain SEM observation images so that the total number of crystal particles observed in two or more, preferably three to five, SEM observation images is the above-mentioned number of crystal particles. Examples of conditions for SEM observation include the following conditions. Accelerating voltage: 15kV Observation magnification: 5000x to 10000x
[0051] Prior to the measurement, the cross section of the sintered body of the measurement sample is mirror-polished to a surface roughness of Ra≦0.02 μm, and then thermally etched for 30 minutes at a temperature 100° C. lower than the sintering temperature.
[0052] Image analysis of the SEM observation image may be performed using image analysis software (e.g., Mac-View Ver. 5, manufactured by MOUNTECH). Specifically, crystal grains in which crystal grain boundaries are observed without interruption in the SEM observation image are extracted, and the area [μm 2 ] is calculated. The diameter [μm] of a circle having the same area is calculated from the calculated area, and the obtained diameter (Heywood diameter; hereafter also referred to as "equivalent circle diameter") can be regarded as the grain size of the crystal grains. The average value of the extracted equivalent circle diameters of the crystal grains can be regarded as the average grain size of the sintered body.
[0053] "Mold density" is the measured density of the molded body [g / cm 3 ] and the volume of the molded product [cm 3 ] is the mass [g] of the molded body obtained by mass measurement using a balance.
[0054] "Density of calcined body" is the measured density of the calcined body [g / cm 3 ] and the volume of the calcined body [cm 3 ] is the mass [g] of the calcined body obtained by mass measurement using a balance.
[0055] "Vickers hardness" is a value measured using a general Vickers tester (e.g., Q30A, manufactured by Qness) equipped with a regular square pyramid indenter made of diamond. The measurement is performed by statically pressing the indenter into the surface of the measurement sample, and measuring the diagonal length of the indentation mark formed on the surface of the measurement sample. The obtained diagonal length can be used to calculate the Vickers hardness from equation (5).
[0056] Hv=F / {d 2 / 2sin(α / 2)} (5)
[0057] In formula (5), Hv is the Vickers hardness (HV), F is the measurement load (1 kgf), d is the diagonal length of the indentation mark (mm), and α is the facing angle of the indenter (136°).
[0058] The Vickers hardness may be measured under the following conditions. Measurement sample: Disc shape with thickness of 3.0±0.5mm Measurement load: 1kgf
[0059] Prior to measurement, the measurement surface of the sample is polished with #800 waterproof abrasive paper to remove irregularities exceeding 0.1 mm as pretreatment.
[0060] The "light transmittance" is the total light transmittance measured in accordance with JIS K 7361-1 for a measurement sample having a thickness of 1 mm. The light transmittance may be measured using a disk-shaped sintered body having a thickness of 1 mm and a surface roughness Ra≦0.02 μm on both sides as a measurement sample, and using a haze meter equipped with a D65 light source as a measurement device (e.g., haze meter NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.).
[0061] "Biaxial bending strength" is a value determined by a two-point bending test in accordance with JIS T 6526. For the measurement of biaxial bending strength, a disk-shaped sintered body having a diameter of 14.5 mm ± 0.5 mm and a thickness of 1.25 mm ± 0.05 mm is used as a measurement sample, and the biaxial bending strength of the sintered body is determined by averaging 10 measurements with a support circle radius of 6 mm and an indenter radius of 0.7 mm.
[0062] The "Weibull modulus" is a value calculated by a method conforming to JIS R 1625. Specifically, a disk-shaped sintered body with a diameter of 14.5 mm ± 0.5 mm and a thickness of 1.25 mm ± 0.05 mm is used as a measurement sample, and the biaxial bending strength is measured 15 times with a support circle radius of 6 mm and an indenter radius of 0.7 mm. The measured strengths are then ranked in ascending order. The nth lowest measured strength σ i σ n For example, the lowest measured intensity σ i is σ1, the second lowest measured intensity σi is σ2,... the 15th lowest measured intensity σ i is σ 15 Next, using the data ranked in ascending order, we calculate ln(1 / ln(1-F i ) on the vertical axis, and ln(σ i ) on the horizontal axis to obtain a regression line, and the slope of the regression line is taken as the Weibull coefficient. Here, i is the rank when ranked in ascending order, σ i is the measured intensity and F i is the cumulative failure probability, F i can be calculated by the following formula: In the formula, N is the number of measurement samples.
[0063] {F i = (i-0.3) / (N+0.4)}
[0064] "Normal pressure sintering" is a method of sintering by heating the material to be sintered (such as a compact or calcined body) without applying an external force. "Sintering temperature" is the maximum temperature reached during sintering, and "sintering time" is the time during which the sintering temperature is maintained.
[0065] The powder composition of the present embodiment includes two or more stabilized zirconias having different contents of stabilizing elements, the content of the stabilizing elements in the powder composition is more than 4.0 mol% and not more than 5.8 mol%, and the rate of change in thermal shrinkage rate per unit temperature at 1300°C is 0.07%°C or less. ―1 and the content of the stabilizing element of each of the two or more stabilized zirconias is 8.0 mol % or less. The powder composition may be a powder composition of stabilized zirconia. From the viewpoint of sufficiently increasing the light transmittance of the sintered body, the total ratio of the two or more stabilized zirconias in the powder composition may be 90 mass % or more, 95 mass % or more, or 98 mass % or more, and may be 100 mass % or less, or less than 100 mass %.
[0066] The powder composition of this embodiment includes a first stabilized zirconia and a second stabilized zirconia, each of which has a stabilizing element content of 8.0 mol% or less. The first stabilized zirconia and the second stabilized zirconia have different stabilizing element contents. For example, the stabilizing element contents of the first stabilized zirconia and the second stabilized zirconia may each be 8.0 mol% or less. The stabilizing element content relative to the total of the first stabilized zirconia and the second stabilized zirconia may be more than 4.0 mol% and 5.8 mol% or less. The rate of change of the thermal shrinkage rate per unit temperature of the powder composition at 1300°C is 0.02%°C. ―1 It may be more than that.
[0067] The powder composition of this embodiment contains two or more stabilized zirconias (for example, a first stabilized zirconia and a second stabilized zirconia) with different stabilizing element contents (hereinafter, the stabilizing element content is also referred to as the "stabilizing element amount", and when the stabilizing element is yttrium or the like, it is also referred to as the "yttrium amount", etc.). This results in a powder composition in which particles (powder particles) with different surface activities coexist. A powder composition that does not contain stabilized zirconias with different stabilizing element amounts is, assuming that ΔV 1300 Even if the above requirement (described later) is satisfied, a sintered body having a translucency suitable for a front denture cannot be obtained by short-time sintering.
[0068] The fact that the powder composition of this embodiment contains two or more stabilized zirconias having different amounts of stabilizing elements can be confirmed by STEM-EDS of the powder composition.
[0069] When a powder composition not including stabilizing zirconia having different amounts of stabilizing elements is measured by STEM-EDS, the distribution width of the stabilizing element amount of the powder particles is less than ±1.0 mol% (i.e., the difference between the maximum value and the minimum value of the stabilizing element amount of the powder particles is less than 2.0 mol%). In this case, the distribution shape of the stabilizing element amount may be monodisperse. In contrast, the powder composition of this embodiment has at least one of the following: the distribution width of the stabilizing element amount is ±1.0 mol% or more (i.e., the difference between the maximum value and the minimum value of the stabilizing element amount of the powder particles is 2.0 mol% or more), and the distribution shape of the stabilizing element amount is multimodal (e.g., bimodal). In the powder composition of this embodiment, it is preferable that the distribution width of the stabilizing element amount of the powder particles is ±1.0 mol% or more, and the distribution shape of the stabilizing element amount is multimodal. In addition, it is preferable that the distribution shape of the stabilizing element amount distribution of the powder composition of this embodiment is bimodal.
[0070] The STEM-EDS measurement may be performed from the TEM observation image and the STEM-EDS element map of the powder composition. That is, zirconia powder particles that are observed in the TEM observation image without overlapping with each other are selected. The number of powder particles to be selected may be 20±10, and multiple TEM observation images (e.g., 3±2) may be used. For the selected powder particles, the EDS spectrum of each measurement point of the STEM-EDS element map is integrated to obtain the EDS spectrum of the powder particle.
[0071] Next, the molar ratio (molar ratio) of the stabilizing element to the total of zirconium and the stabilizing element is calculated from the peak intensity of zirconium and the peak intensity of the stabilizing element using the relative sensitivity coefficient for the obtained EDS spectrum. Since the relative sensitivity coefficient is a value specific to the STEM-EDS device, the value for the STEM-EDS device used for the measurement may be used. This value can also be confirmed by the manual of the device. The amount of the stabilizing element is obtained by converting zirconium and the stabilizing element to their oxides using the obtained molar ratio. The amount of the stabilizing element is the molar ratio (mol%) of the stabilizing element converted into an oxide to the total of zirconium converted into an oxide and the stabilizing element converted into an oxide.
[0072] For example, when the stabilizing element is yttrium, the zirconium (Zr) peak intensity and the yttrium (Y) peak intensity of the powder particles are obtained, and the ratio of the yttrium peak intensity to the zirconium peak intensity is calculated. From the obtained ratio of the yttrium peak intensity to the zirconium peak intensity, the relative sensitivity coefficient is used to correct and obtain the molar ratio of yttrium to zirconium. Using the obtained molar ratio, zirconium and yttrium are converted to oxides, respectively. In this way, the amount of yttrium in the powder particles, that is, the molar ratio [mol%] of yttrium converted to Y2O3 to the total of zirconium converted to ZrO2 and yttrium converted to Y2O3 of the powder particles, may be obtained. The amount of the stabilizing element in a sufficient number of zirconia powder particles (for example, 20±10 particles) may be obtained, and the difference between the maximum value and the minimum value may be used as the distribution width of the amount of the stabilizing element in the powder composition. The distribution shape of the amount of the stabilizing element may be confirmed by a graph or a histogram plotting the relationship between the amount of the stabilizing element in the powder particles and the frequency of the powder particles having the amount of the stabilizing element.
[0073] In this embodiment, the STEM-EDS measurement may be performed using a general transmission electron microscope (e.g., TEM: JEM-2100F, manufactured by JEOL Ltd.) and an energy dispersive X-ray spectrometer (e.g., JED-2300T, manufactured by JEOL Ltd.). The TEM observation conditions include the following conditions.
[0074] Accelerating voltage: 200kV Observation magnification: 50,000x to 500,0000x
[0075] As a pretreatment, the powder composition is crushed in a mortar, and then the powder from which any slow agglomerates have been removed by a dispersion treatment such as ultrasonic treatment is dispersed in acetone to form a slurry, which is then dried on a collodion film.
[0076] Figures 1 and 2 are examples of TEM observation images used in STEM-EDS measurements. As shown in Figures 1 and 2, the amount of stabilizing elements can be determined by performing measurements in the areas surrounded by curves of each powder particle observed without overlapping. The three-digit numbers in Figures 1 and 2 are numbering. If necessary, multiple TEM observation images can be used to measure the composition of 20±10 powder particles.
[0077] In this way, the powder composition of the present embodiment can be confirmed to contain two or more stabilized zirconias with different amounts of stabilizing elements, based on the fact that the difference (distribution width) between the maximum and minimum values of the stabilizing element content of the zirconia powder particles measured in the STEM-EDS measurement is 2.0 mol% or more (the distribution width of the stabilizing element content is the median ±1.0 mol% or more). For example, in the STEM-EDS measurement of the powder composition, when the minimum value of the stabilizing element content is 2 mol% and the maximum value is 5 mol%, the stabilizing element content of the first stabilized zirconia is 2 mol% and the stabilizing element content of the second stabilized zirconia is 5 mol%, and the difference in the stabilizing element content is 3 mol%. Therefore, it can be confirmed that the powder composition contains two or more stabilized zirconias with different amounts of stabilizing elements.
[0078] In addition, it is preferable that the powder composition of this embodiment has stabilized zirconia particles with different amounts of stabilizing elements uniformly dispersed (i.e., the first stabilized zirconia and the second stabilized zirconia are uniformly distributed). For example, it is preferable that a plurality of stabilized zirconia particles with different amounts of stabilizing elements are distributed with high uniformity. Whether or not the particles are uniform can be evaluated by repeatedly measuring the amount of the stabilizing element by STEM-EDS measurement multiple times (e.g., three or more times) using different TEM observation patterns and determining the variation in the difference between the maximum and minimum values of the amount of the stabilizing element obtained in each measurement. That is, when the variation in the difference between the maximum and minimum values of the measured values of the amount of the stabilizing element obtained by STEM-EDS measurement (the variation in multiple measurements) is sufficiently small (e.g., less than ±1 mol%, or even less than ±0.8 mol%), it can be considered that the particles are uniformly distributed.
[0079] The powder composition of the present embodiment may be a powder composition containing two or more types of stabilized zirconia having different stabilizing element contents, or may be a powder composition containing two types of stabilized zirconia having different stabilizing element contents. Also, it may be a powder composition containing two or more types of stabilized zirconia powder having different stabilizing element contents, or may be a powder composition containing two types of stabilized zirconia powder having different stabilizing element contents. Also, it may be a stabilized zirconia powder composition containing a first stabilized zirconia and a second stabilized zirconia, or may be a zirconia powder composition containing a first stabilized zirconia powder and a second stabilized zirconia powder. Also, it may be a mixture of two or more types of stabilized zirconia powder having different stabilizing element contents.
[0080] In order to finely adjust the amount of the stabilizing element in the powder composition, the powder composition of this embodiment may contain 3 or more, 4 or more, or 6 or less, or 5 or less stabilized zirconias (e.g., particles) having different stabilizing element contents. When containing three or more stabilized zirconias, it is sufficient to contain three or more stabilized zirconias having different stabilizing element contents, and it is preferable that the three stabilized zirconias each have a different stabilizing element content.
[0081] The amount of the stabilizing element in each stabilized zirconia contained in the powder composition of this embodiment is 8.0 mol% or less. For example, when the powder composition contains the first stabilized zirconia and the second stabilized zirconia, the amount of the stabilizing element in each of the first stabilized zirconia and the second stabilized zirconia is 8.0 mol% or less. That is, the powder composition of this embodiment does not contain stabilized zirconia having a stabilizing element amount of more than 8.0 mol% (the stabilizing element content of the first stabilized zirconia and the second stabilized zirconia is 8.0 mol% or less). In order to obtain a powder composition more suitable for short-time sintering, it is preferable that the powder composition of this embodiment does not contain stabilized zirconia having a stabilizing element amount of more than 8.0 mol%, and further, does not contain stabilized zirconia having a stabilizing element amount of 8.0 mol% or more, or even 7.5 mol% or more. A powder composition containing stabilized zirconia having a stabilizing element amount of more than 8.0 mol% has a stabilizing element amount of 8.0 mol% or less, and the stabilizing element amount of 8.0 mol% or less is 8.0 mol% or less. If ΔV 1300 Even if the above requirement (described later) is satisfied, a sintered body having a translucency suitable for a front denture cannot be obtained by short-time sintering.
[0082] The powder composition of this embodiment preferably contains a first stabilized zirconia having a stabilizing element content of 1.0 mol% or more and 5.0 mol% or less, and a second stabilized zirconia having a stabilizing element content of 3.0 mol% or more and 8.0 mol% or less. The first stabilized zirconia and the second stabilized zirconia may be stabilized zirconia powders having different stabilizing element contents. In the powder composition of this embodiment, the stabilized zirconia having a low stabilizing element content is referred to as the "first stabilized zirconia", and the stabilized zirconia having a high stabilizing element content is referred to as the "second stabilized zirconia". The terms "first" and "second" are used to conveniently distinguish between two stabilized zirconias having different stabilizing element contents, and do not mean any permutation or the like.
[0083] The first stabilized zirconia (stabilized zirconia having a low content of stabilizing elements) preferably has a stabilizing element content of 1.0 mol% or more, 1.3 mol% or more, 1.5 mol% or more, 1.8 mol% or more, 2.0 mol% or more, or 2.3 mol% or more, and 5.0 mol% or less, 4.5 mol% or less, 4.2 mol% or less, 4.0 mol% or less, or 3.5 mol% or less.
[0084] The second stabilized zirconia (stabilized zirconia having a high content of stabilizing elements) preferably has a stabilizing element content of 3.0 mol% or more, 3.5 mol% or more, 4.0 mol%, 4.5 mol% or more, or 5.0 mol% or more, and 8.0 mol% or less, 7.5 mol% or less, 7.0 mol% or less, 6.8 mol%, 6.5 mol% or less, or 6.3 mol% or less. By including the first stabilized zirconia having a small ΔV in the first half of sintering and the second stabilized zirconia having a large ΔV in the first half of sintering, the powder composition has a ΔV that exerts a synergistic effect of the first stabilized zirconia and the second stabilized zirconia. As a result, even though the amount of stabilizing elements as a powder composition is high, the ΔV of the powder composition in the first half of sintering is easily suppressed.
[0085] By decreasing the content of the stabilizing element in the first stabilized zirconia or increasing the content of the first stabilized zirconia in the powder composition, it becomes easier to suppress ΔV in the first half of the sintering of the powder composition.
[0086] In order to allow particles (powder particles) with different surface activities to coexist, the first stabilized zirconia and the second stabilized zirconia only need to have different amounts of stabilizing elements.
[0087] The difference in the amount of stabilizing elements between the first stabilized zirconia and the second stabilized zirconia (hereinafter also referred to as the "stabilizing element difference") is preferably 1.5 mol% or more, 2.0 mol% or more, 2.5 mol% or more, or 3.0 mol% or more, and 5.0 mol% or less, 4.5 mol% or less, 4.0 mol% or less, or 3.5 mol% or less.
[0088] The ratio of the first stabilized zirconia and the second stabilized zirconia contained in the powder composition of this embodiment is arbitrary as long as it satisfies the above-mentioned configuration, and examples of the first stabilized zirconia:second stabilized zirconia ratio include 1% by mass:99 to 99% by mass:1% by mass, 20% by mass:80 to 80% by mass:20% by mass, or 35% by mass:65 to 65% by mass:35% by mass, and 45% by mass:55 to 55% by mass:45% by mass.
[0089] The first stabilized zirconia and the second stabilized zirconia may each be powder particles. That is, the powder composition may include first stabilized zirconia particles and second stabilized zirconia particles. The powder composition may include three or more types of stabilized zirconia (stabilized zirconia particles).
[0090] Since densification during short-time sintering is likely to be promoted, the BET specific surface area of the first stabilized zirconia is preferably equal to or greater than the BET specific surface area of the second stabilized zirconia, and the BET specific surface area of the first stabilized zirconia is preferably 0.05 to 1.0 m2 less than the BET specific surface area of the second stabilized zirconia. 2 / g or more, even 1.5m 2 / g or more, or even 2.0m 2 It is not necessary to make the difference in the BET specific surface area larger than necessary. For example, the difference between the BET specific surface area of the first stabilized zirconia and the BET specific surface area of the second stabilized zirconia is preferably 8.0 m 2 / g or less, 6.0m 2 / g or less or 3.5m 2 For example, it can be exemplified as being equal to or less than 1 / g.
[0091] The BET specific surface area of the first stabilized zirconia is 8 m 2 / g or more, 10m 2 / g or more, 12m 2 / g or more, 14m 2 / g or more, and 16m 2 / g or less or 15m 2 For example, it can be exemplified as being equal to or less than 1 / g.
[0092] The amount of the stabilizing element in the powder composition of this embodiment (i.e., the content of the stabilizing element as the powder composition) is more than 4.0 mol% and not more than 5.8 mol%. If the amount of the stabilizing element is 4.0 mol% or less, a sintered body satisfying the translucency required for a front tooth denture cannot be obtained by short-time sintering. On the other hand, if the content of the stabilizing element exceeds 5.8 mol%, it becomes difficult to stably manufacture a sintered body satisfying the translucency required for a front tooth denture by short-time sintering. The amount of the stabilizing element in the powder composition of this embodiment is preferably more than 4.0 mol%, 4.2 mol% or more, 4.4 mol% or more, 4.5 mol% or more, 4.7 mol% or more, 4.8 mol% or more, or 5.0 mol% or more, and is preferably 5.8 mol% or less, 5.7 mol% or less, or 5.5 mol% or less. In this embodiment, the amount of the stabilizing element in the powder composition may be determined by ICP analysis.
[0093] The powder composition of the present embodiment preferably does not contain undissolved stabilizing elements. "Does not contain undissolved stabilizing elements" means that in the above-mentioned XRD measurement and XRD pattern analysis, no XRD peaks derived from compounds of stabilizing elements (e.g., oxides of stabilizing elements such as yttria (Y2O3)) are confirmed, and it is acceptable for the powder composition of the present embodiment to contain undissolved stabilizing elements to the extent that the effect of the powder composition is not impaired.
[0094] The stabilizing element is preferably one or more selected from the group consisting of yttrium (Y), calcium (Ca) and magnesium (Mg). Yttrium, calcium and magnesium function as stabilizing elements without coloring zirconia. The stabilizing element may include yttrium, or may be only yttrium.
[0095] A preferred yttrium amount in the powder composition of this embodiment is greater than 4.0 mol%, 4.2 mol% or more, 4.4 mol% or more, 4.5 mol% or more, 4.7 mol% or more, 4.8 mol% or more, or 5.0 mol% or more, and is 5.8 mol% or less, 5.7 mol% or less, or 5.5 mol% or less.
[0096] In order to finely adjust ΔV, the powder composition of this embodiment may contain one or more additive elements selected from the group consisting of aluminum, germanium, silicon, and lanthanum, may contain one or more additive elements selected from the group consisting of aluminum, germanium, and silicon, may contain one or more additive elements selected from the group consisting of aluminum and germanium, and may contain aluminum. When the powder composition of this embodiment contains an additive element, it may be considered as a powder composition containing the additive element and having zirconia containing a stabilizing element as a matrix. The additive element may be contained in the powder composition as an oxide. Note that the powder composition of this embodiment may not contain the additive element (i.e., the content of the additive element may be equal to or less than the measurement limit of composition analysis).
[0097] The content of the added element calculated as an oxide (hereinafter also referred to as the "added element amount", and when the added element is aluminum, etc., the amount of the added element is also referred to as the "aluminum amount", etc.) can be, for example, 0 mass% or more, more than 0 mass% or 0.001 mass% or more, and less than 0.2 mass%, 0.1 mass% or less, less than 0.05 mass%, 0.03 mass% or less, 0.01 mass% or less, or 0.005 mass% or less.
[0098] For example, in a composition containing yttrium as a stabilizing element, aluminum as an additive element, and zirconia as a matrix, the amount of the stabilizing element (amount of yttrium) is the molar ratio [mol%] of yttrium converted into Y2O3 relative to the total of zirconium converted into ZrO2 and yttrium converted into Y2O3, and is calculated by {Y2O3 [mol] / (ZrO2+Y2O3) [mol]} × 100. The amount of additive element (amount of aluminum) in the composition is the mass ratio [mass%] of aluminum converted into Al2O3 relative to the total of zirconium converted into ZrO2, yttrium converted into Y2O3, and aluminum converted into Al2O3, and is calculated by the following formula. {Al2O3[g] / (ZrO2+Y2O3+Al2O3)[g]}×100
[0099] The powder composition of the present embodiment may contain an element having a function of coloring zirconia (hereinafter, also referred to as a "coloring element") within a range that does not impair the effect of the powder composition. The coloring element may be an element having a function of suppressing the phase transformation of zirconia, or may be an element having no function of suppressing the phase transformation of zirconia. Specific examples of the coloring element include at least one of transition metal elements and lanthanoid rare earth elements, and further at least one of transition metal elements other than zirconium and hafnium and lanthanoid rare earth elements other than lanthanum, and preferably at least one selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), titanium (Ti), vanadium (V), praseodymium (Pr), neodymium (Nd), europium (Eu), gadolinium (Gd), terbium (Tb), erbium (Er) and ytterbium (Yb), further at least one selected from the group consisting of iron, cobalt, manganese, titanium, praseodymium, neodymium, terbium and erbium, and further at least one selected from the group consisting of iron, cobalt, titanium, terbium and erbium.
[0100] The powder composition of this embodiment may contain inevitable impurities such as hafnia (HfO2). The content of hafnia as an inevitable impurity varies greatly depending on the raw material ore and the manufacturing method, but can be, for example, 2.0 mass% or less. In this embodiment, calculation of values related to the composition, such as the content and density, may be performed by regarding hafnia as zirconia (ZrO2).
[0101] The rate of change in thermal shrinkage rate per unit temperature at 1300°C of the powder composition of this embodiment (hereinafter referred to as "ΔV 1300 " is also called ".) is 0.07%℃ -1 Less than 0.07%℃ -1 Less than 0.065%℃ -1 or less than 0.06%℃ -1 In addition to the above configuration, it is preferable that ΔV 1300By satisfying the above condition, even if the powder composition of the present embodiment is sintered for a short time, a sintered body having a translucency suitable for a front denture can be obtained. Note that 1300°C is a temperature range in which the thermal contraction of zirconia progresses. Therefore, ΔV 1300 is 0%℃ -1 and even more than 0.02%℃ -1 Above 0.04%℃ -1 or above 0.05%℃ -1 The above points can be mentioned.
[0102] The rate of change in the thermal shrinkage rate per unit temperature at 1500° C. of the powder composition of this embodiment (hereinafter referred to as “ΔV 1500 " is also called ". -1 or above 0.03%℃ -1 This makes it easier to promote densification during short-time sintering. 1500 is 0.05%℃ -1 Less than or equal to 0.04%℃ -1 The following are some of the reasons: ΔV 1500 is 0.05%℃ -1 When the powder composition is sintered for a short period of time, a sintered body having high light-transmitting properties can be stably obtained by sintering the powder composition within the range of 0.1 to 1.0 mm.
[0103] It is easier to have suitable sintering properties for short-time sintering, so ΔV 1300 and ΔV 1500 It is preferable that ΔV is different, that is, the rate of change of the thermal shrinkage rate is not constant. 1300 is ΔV 1500 It is larger than (ΔV 1300 >ΔV 1500 It is preferable that the relationship between the (ΔV 1300 -ΔV 1500 ) is 0.05%℃ -1 Below that, 0.045%℃ -1 Also, ΔV 1300 -ΔV 1500 is 0%℃ -1 Above 0%℃ -1 More than or even 0.010%℃ -1 or even 0.020%℃-1 More preferably, it is equal to or greater than this.
[0104] ΔV 1300 and ΔV 1500 is indirectly affected by the composition of the powder composition. For example, a decrease (or increase) in the amount of stabilizing elements and a decrease (or increase) in the amount of added elements causes ΔV 1300 In addition, the decrease (or increase) in the BET specific surface area of the first stabilized zirconia or the decrease (or increase) in the amount of the stabilizing element tends to slow (or speed up). 1300 In addition, the decrease (or increase) in the BET specific surface area of the second stabilized zirconia leads to a decrease (or increase) in ΔV 1500 tends to be faster (or slower). By adjusting these, ΔV 1300 and ΔV 1500 can be appropriately controlled.
[0105] The powder composition of this embodiment has a BET specific surface area of 8 m 2 / g or more 13m 2 / g or less. In the amount of the stabilizing element in the powder composition of this embodiment, when the BET specific surface area satisfies this range, the above-mentioned ΔV 1300 The BET specific surface area is 8m 2 / g or more, 9m 2 / g or more, 9.5m 2 / g or more or 10m 2 / g or more, and 13m 2 / g or less, 12m 2 / g or less or 11m 2 It is preferable that the molecular weight is not more than 1 / g.
[0106] The T+C phase ratio of the powder composition of this embodiment is preferably 65% or more, 75% or more, 80% or more, or 90% or more. Also, the T+C phase ratio is preferably 95% or less, or 93% or less.
[0107] The average particle size of the powder composition of this embodiment is preferably 0.35 μm or more, more preferably 0.40 μm or more, and more preferably 0.50 μm or less, or 0.45 μm or less.
[0108] In order to improve flowability, the powder composition of the present embodiment may be a granular powder. The average granular particle size of the granular powder is, for example, 30 μm or more, 40 μm or more, or 50 μm or more, and 80 μm or less, or 60 μm or less. The bulk density of the granular powder is, for example, 1.00 g / cm. 3 or more than 1.10g / cm 3 More than 1.40g / cm 3 Less than or equal to 1.30g / cm 3 The following are some of the reasons:
[0109] A method for producing the powder composition of this embodiment will be described.
[0110] The powder composition of the present embodiment may be produced by any method as long as it has the above-mentioned characteristics. A preferred method for producing the powder composition of the present embodiment includes a method for producing a powder composition comprising a step of mixing two or more stabilized zirconia powders having different contents of stabilizing elements.
[0111] The stabilized zirconia powder subjected to the process of mixing two or more stabilized zirconia powders having different stabilizing element contents (hereinafter also referred to as the "mixing process") may be, for example, the first stabilized zirconia powder and the second stabilized zirconia powder described above.
[0112] Each stabilized zirconia powder preferably has a BET specific surface area similar to that of the powder composition of this embodiment. In addition, it is more preferable that the BET specific surface areas of the stabilized zirconia powders are different from each other. It is even more preferable that the BET specific surface area of the first stabilized zirconia powder is equal to or greater than the BET specific surface area of the second stabilized zirconia powder. Specifically, the BET specific surface area of the first stabilized zirconia powder is, for example, 0 m2 smaller than the BET specific surface area of the second stabilized zirconia powder. 2 / g or more, preferably 1.5m 2 / g or more, more preferably 2.0m 2The difference between the BET specific surface area of the first stabilized zirconia powder and the BET specific surface area of the second stabilized zirconia powder is 6.0 m 2 / g or less, and 2 / g or less.
[0113] When the amount of the stabilizing element in each stabilized zirconia powder used as a starting material in the manufacturing method of the powder composition is known, instead of the above-mentioned STEM-EDS measurement, the amount of the stabilizing element in each stabilized zirconia powder contained in the powder composition may be calculated from the amount of the stabilizing element and the mixing ratio of each stabilized zirconia powder.
[0114] The difference between the maximum and minimum values of the amount of the stabilizing element obtained by STEM-EDS measurement (distribution width, method I) tends to be larger than the difference between the amount of the stabilizing element of each powder of stabilized zirconia (method II). This is because the difference in method II is obtained as the difference between the average values of the amount of the stabilizing element of each powder, while the difference in method I is obtained as the maximum and minimum values in the mixture of each powder. If at least one of the differences obtained by each of methods I and II is 2.0 mol% or more, it can be determined that two or more types of stabilized zirconia having different amounts of the stabilizing element are contained. At least one of the differences obtained by each of methods I and II may be 2.5 mol% or more, more than 2.5 mol%, or 3.0 mol% or more. This allows the light transmittance and biaxial bending strength of the obtained sintered body to be sufficiently high. At least one of the differences obtained by each of methods I and II may be 6.0 mol% or less, 5.0 mol% or less, or 4.0 mol% or less. At least one of the differences determined by each of Method I and Method II may be 2.0 to 6.0 mol %. The upper and / or lower limits of the numerical ranges can be replaced with the numerical values described above.
[0115] The stabilized zirconia powder to be subjected to the mixing step may be produced by any method, including, for example, a powder calcination step of heat-treating a composition containing a zirconia sol and a stabilizing element source (hereinafter also referred to as a "sol composition") to obtain a calcined powder, and a powder grinding step of grinding the calcined powder.
[0116] The zirconia sol is a sol in which zirconium dioxide is hydrated and crosslinked, and is preferably a zirconia sol obtained by at least one of a hydrothermal synthesis method and a hydrolysis method, and more preferably a zirconia sol obtained by a hydrolysis method.
[0117] The stabilizing element source (hereinafter, when the stabilizing element is yttrium, etc., it may be referred to as "yttrium source" etc.) as long as it is a compound containing a stabilizing element, and may be at least one selected from the group consisting of oxide, hydroxide, oxyhydroxide, halide, sulfate, nitrate and acetate of the stabilizing element, preferably at least one of oxide, hydroxide, oxyhydroxide and chloride of the stabilizing element, more preferably at least one of oxide, hydroxide and chloride of the stabilizing element. For example, the yttrium source may be at least one selected from the group consisting of yttrium oxide (yttria), yttrium hydroxide and yttrium chloride, preferably at least one of yttrium oxide and yttrium chloride.
[0118] The content of the stabilizing element source may be the same as the amount of the stabilizing element in the desired stabilized zirconia, and may be the same as the amount of the stabilizing element described above.
[0119] The sol composition may contain a zirconia sol and a stabilizing element source, and an example of the sol composition is an aqueous solution containing a zirconia sol and a stabilizing element source.
[0120] In the powder calcination step, the sol composition is heat-treated to obtain a calcined powder, which is a precursor of the stabilized zirconia powder.
[0121] In the heat treatment in the powder calcination step, the heat treatment conditions may be appropriately set according to the amount of the sol composition to be subjected to the powder calcination step, the BET specific surface area of the calcined powder to be targeted, and the characteristics of the calcination furnace to be used for calcination. For example, the higher (or lower) the heat treatment temperature, the lower (or the higher) the BET specific surface area tends to be. The heat treatment temperature is, for example, 950°C or higher, 1000°C or higher, 1020°C or higher, or 1100°C or higher, and 1250°C or lower, 1200°C or lower, 1180°C or lower, or 1150°C or lower. The holding time at the heat treatment temperature may be, for example, 1 hour or more and 8 hours or less, or even 2 hours or more and 6 hours or less. However, the holding time has little effect on the BET specific surface area of the calcined powder compared to the heat treatment temperature. The heat treatment may be performed using a general calcination furnace.
[0122] The heat treatment may be performed in any atmosphere, including at least one selected from the group consisting of an oxidizing atmosphere, a reducing atmosphere, an inert atmosphere, and a vacuum atmosphere. An oxidizing atmosphere is preferable, and an air atmosphere is more preferable.
[0123] In the powder grinding step, the grinding method may be any method that can obtain a powder having a desired particle size. The grinding method may be at least one of wet grinding and dry grinding, and wet grinding is preferred. A preferred grinding method is ball mill grinding. The grinding conditions may be appropriately set according to the grinding method and the desired particle size. For example, the particle size tends to be smaller by increasing the grinding time.
[0124] In the manufacturing method of this embodiment, two or more stabilized zirconia powders having different contents of stabilizing elements are mixed in the mixing step. The mixing method may be any method that can uniformly mix the stabilized zirconia powders, and may be at least one of dry mixing and wet mixing, with wet mixing being preferred, and mixing in an aqueous solvent being more preferred.
[0125] A preferred mixing method, which allows the stabilized zirconia powder to be mixed uniformly, is to prepare a slurry containing the stabilized zirconia powder and mix this.
[0126] In addition, a method of adding a slurry containing a stabilized zirconia powder having a large BET specific surface area to a slurry containing a stabilized zirconia powder having a small BET specific surface area and mixing them can be used. By using such a mixing method, the slurry containing the stabilized zirconia powder can be easily mixed uniformly, and it becomes easier to satisfy ΔV suitable for short-time sintering.
[0127] Mixing requires a stirring power of 0.005kW / m 3 or more than 0.01kW / m 3 It is sufficient if it is more than 0.1kW / m 3 or more than 0.3kW / m 3 It is preferable that the required stirring power is 1.0 kW / m or more. By mixing with the application of such a required stirring power, it becomes easier to suppress the variation in properties when the powder composition of this embodiment is repeatedly produced. This makes it easier to increase the Weibull coefficient of the sintered body obtained by sintering the powder composition in a short time. The required stirring power does not need to be higher than necessary, and is preferably 1.0 kW / m 3 Less than or equal to 0.7kW / m 3 The following can be exemplified.
[0128] The mixing time may be appropriately set depending on the amount of powder to be subjected to the mixing step, and may be, for example, from 0.5 hours to 12 hours.
[0129] The mixing ratio of the stabilized zirconia powder may be adjusted appropriately depending on the amount of stabilizing elements in the stabilized zirconia and the desired powder composition, and examples of the mixing ratio of the first stabilized zirconia powder:the second stabilized zirconia powder may be 1% by mass:99 to 99% by mass:1% by mass, 20% by mass:80 to 80% by mass:20% by mass, or 35% by mass:65 to 65% by mass:35% by mass, or 45% by mass:55 to 55% by mass:45% by mass.
[0130] In order to finely adjust the amount of the stabilizing element in the powder composition, three or more, four or more, and up to six or five types of stabilizing zirconia having different amounts of the stabilizing element may be mixed in the mixing step.
[0131] In the mixing step, an additive element source may be further mixed. This results in a powder composition containing the additive element. The additive element source (hereinafter, when the additive element is aluminum, etc., it may also be referred to as an "aluminum source" or the like) is at least one of the additive element and its compound, preferably at least one of the oxide of the additive element and its precursor, and more preferably the oxide of the additive element. For example, the aluminum source is at least one of alumina and its precursor, preferably alumina, and more preferably α-alumina.
[0132] The amount of the additive element source to be mixed may be the same as the amount of the additive element in the desired powder composition, and may be the same as the amount of the additive element described above.
[0133] In the mixing step, a coloring element source may be further mixed. The coloring element source is a compound containing a coloring element, preferably at least one of an oxide of the coloring element and a precursor thereof, more preferably an oxide of the coloring element. The amount of the coloring element source to be mixed may be an amount that provides the desired color tone of the sintered body.
[0134] In the mixing step, in addition to mixing at least one of an additive element source and a coloring element source (hereinafter also referred to as "additive element source, etc."), or instead of mixing the additive element source, etc., stabilized zirconia containing at least one of an additive element and a coloring element may be provided.
[0135] The manufacturing method of this embodiment may include a granulation step of granulating the powder composition after the mixing step. The granulation may be performed by any method that can cause the zirconia powder to be in a slowly aggregated state, and examples of the granulation method include a granulation method such as spray granulation.
[0136] In the granulation step, the powder composition of the present embodiment may be mixed with a binder and granulated. By including a binder, the shape retention of the molded body obtained by molding the granular powder is increased. The binder contained in the granular powder may be a known one used in molding ceramics, and is preferably an organic binder. The organic binder is one or more selected from the group of polyvinyl alcohol, polyvinyl butyrate, wax, and acrylic resin, preferably one or more of polyvinyl alcohol and acrylic resin, and more preferably acrylic resin. In the present embodiment, the acrylic resin is a polymer containing at least one of an acrylic acid ester and a methacrylic acid ester. Specific examples of the acrylic resin include one or more selected from the group of polyacrylic acid, polymethacrylic acid, acrylic acid copolymer, and methacrylic acid copolymer, and derivatives thereof.
[0137] Next, the calcined body of the present disclosure will be described with reference to an example of an embodiment.
[0138] The calcined body of the present embodiment includes two or more stabilized zirconias having different contents of stabilizing elements, the content of the stabilizing elements in the calcined body is more than 4.0 mol% and not more than 5.8 mol%, and the rate of change in thermal shrinkage rate per unit temperature at 1300°C is 0.07%°C or less. ―1 and the content of each of the stabilizing elements of the two or more stabilized zirconias is 8.0 mol % or less. The calcined body may be a calcined body of stabilized zirconia. From the viewpoint of sufficiently increasing the light transmittance of the sintered body, the total ratio of the two or more stabilized zirconias in the calcined body may be 90 mass % or more, 95 mass % or more, or 98 mass % or more, and may be 100 mass % or less or less than 100 mass %. With the calcined body of this embodiment, a sintered body that satisfies the translucency required for a front tooth denture can be obtained even by short-time sintering.
[0139] The calcined body of this embodiment may contain a first stabilized zirconia and a second stabilized zirconia each having a stabilizing element content of 8.0 mol% or less. The first stabilized zirconia and the second stabilized zirconia have different stabilizing element contents. For example, the stabilizing element contents of the first stabilized zirconia and the second stabilized zirconia may each be 8.0 mol% or less. The stabilizing element content in the calcined body may be more than 4.0 mol% and 5.8 mol% or less. The rate of change in thermal shrinkage rate per unit temperature of the calcined body at 1300°C is 0.02%°C. ―1 It may be more than that.
[0140] The calcined body of this embodiment contains two or more stabilized zirconias with different stabilizing element contents. The fact that the calcined body of this embodiment contains two or more stabilized zirconias with different stabilizing element contents can be measured by STEM-EDS in the same manner as for the powder composition of this embodiment, except that a powder obtained by dry-pulverizing the calcined body so that the average particle size is 0.40 μm or more and 0.50 μm or less is used. The calcined body having at least one of a distribution width of the stabilizing element amount of ±1.5 mol% or more and a multimodal (e.g., bimodal) distribution shape of the stabilizing element amount contains two or more stabilized zirconias with different stabilizing element amounts. It is preferable that the calcined body of this embodiment has a bimodal distribution shape in the stabilizing element amount distribution.
[0141] The BET specific surface area of the calcined body of this embodiment is 5 m 2 / g or more or 6m 2 / g or more, and 2 / g or less or 7m 2 It is preferable that the molecular weight is not more than 1 / g.
[0142] The T+C phase ratio of the calcined body of this embodiment is preferably 75% or more, 80% or more, 90% or more, 95% or more, or 98% or more, and is preferably 100% or less, or 99% or less.
[0143] The calcined body density of the present embodiment is 2.95 g / cm 3or more than 3.00g / cm 3 or more and 3.50 g / cm 3 Below, 3.30g / cm 3 Less than or equal to 3.15g / cm 3 The following are some of the reasons:
[0144] In order to prevent defects from occurring during shaping processing such as CAM processing, the Vickers hardness of the calcined body of this embodiment is 35 kgf / mm 2 or more than 40kgf / mm 2 More than 100kgf / mm 2 Below, 80kgf / mm 2 Below, 70kgf / mm 2 Below, 55kgf / mm 2 Below, 50kgf / mm 2 or less than 47kgf / mm 2 It is preferable that:
[0145] Other than the fact that the calcined body is composed of fused particles and the points mentioned above, the calcined body of this embodiment has the same features as the powder composition of this embodiment.
[0146] Next, a method for producing the calcined body of this embodiment will be described.
[0147] The method for producing the calcined body of this embodiment is arbitrary, but examples thereof include a method for producing a calcined body having a step of calcining a molded body containing the powder composition of this embodiment.
[0148] The molded body to be subjected to the step of calcining a molded body containing the powder composition of this embodiment (hereinafter also referred to as the "calcination step") is preferably a molded body in a state in which the powder composition of this embodiment is molded.
[0149] The shape of the molded body can be at least one selected from the group consisting of a cube, a rectangular parallelepiped, a polyhedron, a columnar shape, a cylindrical shape, a disk shape, and a substantially spherical shape. The molded body may have a shape similar to that of the intended calcined body or sintered body, such as the shape of a dental prosthesis, taking into consideration thermal shrinkage due to sintering.
[0150] The density of the compact is 2.80 g / cm 3 More than 2.95g / cm 3 or more than 3.00g / cm 3 or more and 3.50 g / cm 3 Below, 3.40g / cm 3 Below, 3.30g / cm 3 Below, 3.20g / cm 3 Less than or equal to 3.15g / cm 3 The following are some of the reasons:
[0151] In this embodiment, the manufacturing method of the molded body is arbitrary, and a known ceramic molding method can be applied. For example, the molding method can be one or more selected from the group consisting of uniaxial pressing, cold isostatic pressing, slip casting, and injection molding. For simplicity, the molding method is preferably at least other than slip casting, and more preferably at least one of uniaxial pressing and cold isostatic pressing, and more preferably cold isostatic pressing is performed after uniaxial pressing. The pressure of the uniaxial pressing can be 15 MPa or more and 150 MPa or less, and the pressure of the cold isostatic pressing can be 90 MPa or more and 400 MPa or less, and the higher the pressure in molding, the higher the density of the molded body tends to be.
[0152] When the molded body contains a binder, a step of removing the binder, i.e., a so-called binder removal step, may be carried out prior to the calcination. Any method for removing the binder may be used, but an example of the method is a heat treatment in the air at 400°C or higher and lower than 900°C.
[0153] The calcination may be performed at a temperature at which zirconia does not sinter. The calcination conditions include the following: Calcination atmosphere: Oxidizing atmosphere, preferably air atmosphere Calcination temperature: 950°C or higher or 1000°C or higher, and 1150℃ or less or 1100℃ or less Calcination time: 0.5 hours or more or 1 hour or more, and 5 hours or less or 3 hours or less
[0154] Next, a method for producing a sintered body using at least one of the powder composition of this embodiment and the calcined body (hereinafter also referred to as "the powder composition of this embodiment, etc.") will be described.
[0155] The powder composition of this embodiment can be calcined to produce a calcined body suitable for a precursor of a front tooth denture. The powder composition of this embodiment can be sintered to produce a sintered body suitable for a front tooth denture. In particular, the powder composition of this embodiment can produce a sintered body having aesthetics based on translucency equivalent to that of a sintered body obtained by a conventional sintering method (e.g., normal sintering) even in the case of short-time sintering.
[0156] In the method for producing a sintered body using the powder composition of the present embodiment, a sintered body is obtained by sintering the powder composition by any sintering method. The sintering in the sintering step can be performed by one or more sintering methods known as a method for sintering ceramics, such as atmospheric sintering, pressure sintering, and vacuum sintering. Since the sintering method is widely applied to the production of dental prosthetic materials, the sintering method is preferably atmospheric sintering, and more preferably, only atmospheric sintering, that is, a sintering method that does not use pressure sintering or vacuum sintering. When the sintering method is only atmospheric sintering, a sintered body is obtained from the powder composition of the present embodiment as a so-called atmospheric sintered body.
[0157] A particularly preferred sintering method is normal pressure sintering in an air atmosphere, and the sintering time is 7 hours or less, preferably 5 hours or less, more preferably 3 hours or less, and even more preferably 1 hour or less. Furthermore, sintering in which the temperature is increased to the sintering temperature at different heating rates (for example, sintering in which the temperature is increased at two heating rates) is preferred.
[0158] As preferred sintering conditions, the following conditions can be exemplified. Sintering method: Pressureless sintering Sintering atmosphere: oxidizing atmosphere, preferably air atmosphere Sintering temperature: 1450°C or higher, 1500°C or higher, or 1550°C or higher, and 1650°C or lower, 1620°C or lower, or 1600°C or lower Sintering time: 3 minutes or more, 5 minutes or more, 7 minutes or more, or 8 minutes or more, and 30 minutes or less, 20 minutes or less, or 15 minutes or less Heating rate: (room temperature to 1050℃) 150°C / min or more, 200°C / min or more, or 250°C / min or more, and 350℃ / min or less or 300℃ / min or less (Sintering temperature from 1050℃) 30°C / min or more, 40°C / min or more, or 50°C / min or more, and 150℃ / min or less, 70℃ / min or less, or 60℃ / min or less Cooling rate: (from sintering temperature to 900℃) 30°C / min or more, 40°C / min or more, or 60°C / min or more, and 300℃ / min or less, 100℃ / min or less, or 65℃ / min or less
[0159] When the powder composition is sintered, the powder composition may be molded into a molded body by any method prior to sintering. When the calcined body is sintered, the calcined body to be sintered may be processed into any shape prior to sintering. The calcined body can be processed into any shape by CAD / CAM or other processing, which makes it easier to obtain a sintered body of any shape.
[0160] Next, as an example of a sintered body obtained by sintering the powder composition of this embodiment, etc., a sintered body obtained by sintering the powder composition of this embodiment for a short period of time (hereinafter also referred to as the "sintered body of this embodiment") will be described below.
[0161] The sintered body of this embodiment is characterized in that it contains stabilized zirconia containing a stabilizing element as a matrix, the content of the stabilizing element is more than 4.0 mol% and not more than 5.8 mol%, the average crystal grain size is 2.5 μm or less, and the tetragonal prime phase ratio is 70% or more. The sintered body may have a stabilizing element content of more than 4.0 mol% and not more than 5.8 mol%, a crystal grain size difference of 0.10 μm or less, and a tetragonal prime phase ratio of 70% or more. The sintered body may be a zirconia sintered body (zirconia sintered body) with zirconia as a matrix.
[0162] The stabilizing element is preferably one or more elements selected from the group consisting of yttrium, calcium and magnesium, and is more preferably yttrium.
[0163] In the sintered body of this embodiment, the stabilizing element is dissolved in zirconia, and preferably, the sintered body of this embodiment does not contain any undissolved stabilizing element.
[0164] The amount of stabilizing elements in the sintered body or matrix is more than 4.0 mol% and not more than 5.8 mol%, and is preferably more than 4.0 mol%, 4.2 mol% or more, 4.4 mol% or more, 4.5 mol% or more, 4.7 mol% or more, 4.8 mol% or more, or 5.0 mol% or more, and is preferably 5.8 mol% or less, 5.7 mol% or less, or 5.5 mol% or less.
[0165] In this embodiment, the amount of the stabilizing element in the sintered body and the matrix may be determined by ICP analysis.
[0166] The average crystal grain size of the sintered body of this embodiment is preferably 2.5 μm or less, 2.0 μm or less, 1.8 μm or less, 1.5 μm or less, 1.3 μm or less, or less than 1.3 μm. The average crystal grain size may be 0.7 μm or more, 0.8 μm or more, 1.0 μm or more, or 1.2 μm or more.
[0167] The crystal grain size difference of the sintered body of this embodiment is 0.10 μm or less, and is preferably less than 0.10 μm, 0.09 μm or less, 0.07 μm or less, 0.05 μm or less, or 0.04 μm or less. The crystal grain size difference may be 0 μm or more or 0.005 μm or more. Such a crystal grain size is considered to be the state of crystal grains obtained by sintering the powder composition of this embodiment for a short time.
[0168] The "crystal grain size difference" is an index showing the state of the crystal grains that make up the sintered body, and more specifically, is an index showing the difference between the crystal grains that make up the surface of the sintered body and the crystal grains that make up the interior of the sintered body.
[0169] The crystal grain size difference can be obtained by image analysis of an SEM observation diagram of a cut surface obtained by cutting the sintered body in the thickness direction. Specifically, first, when the total thickness of the sintered body is taken as 100%, an arbitrary region between the surface and 1% (surface portion) in the thickness direction is observed with an SEM. The SEM observation diagram obtained in this way is image analyzed to obtain the average value of the circle-equivalent diameter of the crystal grains constituting the surface portion of the sintered body (hereinafter referred to as the "surface grain size"). In addition, an arbitrary region between 40% and 60% from the surface in the thickness direction of the sintered body is observed with an SEM. The SEM observation diagram obtained in this way is image analyzed to obtain the average value of the circle-equivalent diameter of the crystal grains constituting the inside of the sintered body (hereinafter referred to as the "internal grain size"). The measured number of crystal grains contained in the surface portion of the sintered body and the number of crystal grains contained in the inside of the sintered body are 450±50 each. If necessary, the circle-equivalent diameter may be measured using multiple SEM observation diagrams. The absolute value of the difference between the surface grain size and the internal grain size obtained in this way is the crystal grain size difference.
[0170] The surface grain size and the internal grain size can be obtained by analysis using image analysis software (for example, Mac-View Ver.5, manufactured by MOUNTECH Co., Ltd.). The absolute value of the difference between the surface grain size and the internal grain size is calculated, and this is taken as the crystal grain size difference.
[0171] The T' phase ratio of the sintered body of the present embodiment is preferably 70% or more, 80% or more, or 90% or more. The T' phase ratio may be 100% or less, or 99% or less.
[0172] The light transmittance of the sintered body of this embodiment is preferably more than 45%, 46% or more, or 47% or more. When the light transmittance has this value, it can be applied to dental prosthetic materials that require particularly high translucency, such as dental prosthetic materials including front dentures. The light transmittance of the sintered body of this embodiment in the range of the amount of stabilizing elements can be, for example, 52% or less, 51% or less, or 50% or less.
[0173] The C-phase ratio of the sintered body of this embodiment is preferably less than 30%, 10% or less, 5% or less, 1% or less, or 0.5% or less. The sintered body of this embodiment may not contain a C phase (the C-phase ratio may be 0%), and the C-phase ratio of the sintered body of this embodiment may be 0% or more.
[0174] The biaxial bending strength of the sintered body of this embodiment is preferably 650 MPa or more, 700 MPa or more, 720 MPa or more, 740 MPa or more, 770 MPa or more, 790 MPa or more, or 800 MPa or more. By satisfying such biaxial bending strength, the sintered body of this embodiment can be applied as a dental prosthesis of a smaller shape. The higher the biaxial bending strength, the more preferable it is. When the stabilizing element amount of this embodiment is satisfied, the biaxial bending strength can be, for example, 1000 MPa or less, 900 MPa or less, 850 MPa or less, or 800 MPa or less.
[0175] The Weibull coefficient of the sintered body of this embodiment can be, for example, 4.0 or more, 5.0 or more, or 6.0 or more. The higher the Weibull coefficient, the more preferable it is, but when the amount of the stabilizing element of this embodiment is satisfied, the Weibull coefficient can be, for example, 15.0 or less, or 12.0 or less.
[0176] Although several embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. For example, the present disclosure also includes a numerical range obtained by arbitrarily combining the upper limit value and the lower limit value specifically described in each of the above-mentioned embodiments. In addition, the present disclosure also includes a range in which the upper limit value and / or the lower limit value are replaced with the values of the examples described below. EXAMPLES
[0177] The present disclosure will be described in detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the examples.
[0178] (Crystal phase, tetragonal + cubic fraction, tetragonal prime fraction, cubic fraction) The crystal phase was identified by XRD measurement using an X-ray diffraction apparatus (apparatus name: Ultima IV, manufactured by RIGAKU Corporation) under the following conditions. Radiation source: CuKα radiation (λ=0.15418nm) Measurement mode: Continuous scan Scan speed: 2° / min Measurement range: 2θ=26°~33° 2θ=72°~76° Acceleration voltage / current: 40mA / 40kV Divergence vertical limit slit: 10mm Divergence / entrance slit: 1° Receiving slit: open Detector: Semiconductor detector (D / teX Ultra) Filter: Ni filter Goniometer radius: 185mm
[0179] The crystalline phases were identified by smoothing and background removal processing using an analysis program attached to the X-ray diffractometer (program name: Integrated Powder X-ray Analysis Software PDXL Ver. 2.2, manufactured by RIGAKU Corporation), and then profile fitting the processed XRD pattern using a split pseudo-Voigt function.
[0180] The tetragonal + cubic crystal fraction, cubic crystal fraction, and tetragonal prime phase fraction were calculated from the XRD patterns of the powder composition, calcined body, and sintered body of the present embodiment using formulas (2), (4), and (3).
[0181] (composition analysis) The composition of the composition was determined by ICP analysis.
[0182] (Stabilizing element amount: Y2O3 [mol%]) The amount of stabilizing elements (mol% of yttrium in terms of oxide) was determined by the above-mentioned method using STEM-EDS measurement of the powder composition or the calcined body. The STEM-EDS measurement was performed using a transmission electron microscope (instrument name: JEM-2100F, manufactured by JEOL Ltd.) and an energy dispersive X-ray spectrometer (instrument name: JED-2300T, manufactured by JEOL Ltd.) under the following conditions. Note that multiple STEM observation images were used so that the number of powder particles measured was 20±10. Accelerating voltage: 200kV Magnification: 400,000x
[0183] As a pretreatment for STEM-EDS measurement, the powder composition was crushed in a mortar. Then, the powder, which had been soft-aggregated by ultrasonic treatment, was dispersed in acetone to prepare a slurry. The slurry was dried on a collodion film to obtain a measurement sample. In the case of the calcined body, the measurement sample was obtained in the same manner as the powder composition, except that the calcined body was dry-pulverized in a mortar.
[0184] (BET specific surface area) The BET specific surface area was measured by the BET multipoint method (5 points) using an automatic specific surface area measuring device (device name: Tristar II 320, manufactured by Shimadzu Corporation) in accordance with JIS R 1626 under the following conditions. Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing in air at 250℃ for 1 hour or more
[0185] (Average particle size) The average particle size was measured by particle size distribution measurement using a Microtrack particle size distribution analyzer (device name: MT3300EXII, manufactured by Microtrack Bell) by laser diffraction / scattering method. The measurement conditions are as follows: Light source: Semiconductor laser (wavelength: 780 nm) Voltage: 3mW Measurement sample: Crushed slurry Refractive index of zirconia: 2.17 Refractive index of solvent (water): 1.333 Calculation mode: HRA
[0186] As a pretreatment, the sample powder was suspended in distilled water to form a slurry, which was then dispersed for 3 minutes using an ultrasonic homogenizer (device name: US-150T, manufactured by Nippon Seiki Seisakusho).
[0187] (Rate of change in thermal shrinkage rate: ΔV) ΔV of the powder composition and the calcined body (ΔV 1300 and ΔV 1500 ) was measured by the above-mentioned method using a thermal dilatometer (device name: TD5000SE, manufactured by NETZSCH) and alumina as a standard sample. Thermal expansion correction of the standard sample was performed using thermal analysis software (software name: Analysis software for TD5000SE Ver.5.0.2, manufactured by NETZSCH).
[0188] The ΔV of the powder composition and the calcined body were measured by the following procedure. Regarding the ΔV of the powder composition, the powder composition was filled into a mold, uniaxially compacted at a pressure of 19.6 MPa, and then subjected to CIP treatment at a pressure of 196 MPa to obtain a cylindrical molded body A with a diameter of 6 mm and a length of 15±2 mm. The molded body A was treated in an air atmosphere at 700° C. for 1 hour to obtain a measurement sample for measuring the ΔV of the powder composition. Regarding the ΔV of the calcined body, the molded body A was calcined at 1000° C. for 1 hour to obtain a measurement sample for measuring the ΔV of the calcined body. The measurement conditions are shown below. Atmosphere: Air flow (100mL / min) Heating rate: 20℃ / min Maximum temperature reached: 1600℃
[0189] T0 was set to 30°C, and the length (l) of the molded body was measured every 3 seconds after the start of the temperature rise. The thermal shrinkage L(T) at each temperature T, including T1 and T2, was calculated from the above formula (1). ΔV 1300 In the measurement, T1 was set to 1300°C and T2 was set to 1303°C. Also, ΔV 1500 In the measurement, T1 was 1500°C and T2 was 1503°C. Tables 2 and 3 show the 1300 and ΔV 1500 The difference was shown.
[0190] (Molded object density) The mass of the compact sample was measured with a balance, and the volume was measured with a vernier caliper to obtain the dimensions. The density of the compact was calculated from the obtained mass and volume.
[0191] (Density of calcined body) The mass of the calcined sample was measured with a balance, and the volume was measured with a vernier caliper to obtain the dimensions. The density of the calcined sample was calculated from the mass and volume obtained.
[0192] (Vickers hardness) The Vickers hardness was measured using a Vickers tester (device name: Q30A, manufactured by Qness) by statically pressing an indenter into the surface of the test sample under the following conditions, and measuring the diagonal length of the indentation mark formed on the surface of the test sample. The diagonal length thus obtained was used to calculate the hardness from Equation (5). Measurement sample: Disc shape with thickness of 3.0±0.5mm Measurement load: 1kgf
[0193] Prior to the measurement, the calcined samples were ground to a depth of 0.1 mm using #800 waterproof abrasive paper.
[0194] (Average grain size and grain size difference) The average crystal grain size and the crystal grain size difference (=|surface grain size-internal grain size|) were determined by the above-mentioned method using a SEM (apparatus name: JSM-IT500LA, manufactured by JEOL Ltd.) and image analysis software (software name: Mac-View Ver.5, manufactured by MOUNTECH Co., Ltd.).
[0195] The conditions for SEM observation were as follows. The average crystal grain size, surface grain size, and internal grain size were determined by measuring 450±50 crystal grains each. For each measurement, multiple SEM observation images were used. Accelerating voltage: 15kV Observation magnification: 5000x
[0196] Prior to the measurement, the cross section of the sintered body of the measurement sample was polished to a surface roughness of Ra≦0.02 μm, and then thermally etched for 30 minutes at a temperature 100° C. lower than the sintering temperature.
[0197] The grain boundaries of the crystal grains were traced on the image analysis software to extract crystal grains with uninterrupted grain boundaries. After extraction, the area and circle equivalent diameter of the crystal grains were obtained using the image analysis software, and the average crystal grain size, as well as the surface grain size and internal grain size were obtained. The absolute value of the difference between the obtained surface grain size and internal grain size was obtained, and the crystal grain size difference was determined. These values were obtained by processing using the image analysis software. For the average crystal grain size and surface grain size, SEM observations of a region 20 μm from the surface of the sintered body (a region of 1% in the thickness direction from the surface of the sintered body) were used, and for the internal grain size, SEM observations of a region 800 μm from the surface of the sintered body (a region of 40% in the thickness direction from the surface of the sintered body) were used.
[0198] (light transmittance) The light transmittance (total light transmittance) was measured using a haze meter (device name: NDH4000, manufactured by Nippon Denshoku Co., Ltd.) with a D65 light source in accordance with a method conforming to JIS K 7361-1. The measurement sample used was a disk-shaped sintered body with a thickness of 1 mm, both sides of which were polished to a surface roughness of Ra ≦ 0.02 μm.
[0199] (Light transmittance ratio) The light transmittance ratio was calculated as the ratio of the light transmittance [%] of the short-time sintered body (described later) to the light transmittance [%] of the normal sintered body (described later).
[0200] (Biaxial bending strength) The biaxial bending strength was measured according to the method of JIS T 6526. The measurement was performed 10 times and the average value was calculated. The measurement was performed on a disk-shaped sintered body sample with a diameter of 14.5 mm ± 0.5 mm and a thickness of 1.25 mm ± 0.05 mm, with a support circle radius of 6 mm and an indenter radius of 0.7 mm. The crosshead speed was 0.5 mm / min.
[0201] (Weibull coefficient) The Weibull modulus was calculated according to the method of JIS R 1625. A circular sintered body with a diameter of 14.5 mm ± 0.5 mm and a thickness of 1.25 mm ± 0.05 mm was used as a measurement sample, and the biaxial bending strength was measured 15 times with a support circle radius of 6 mm and an indenter radius of 0.7 mm, and the Weibull modulus was calculated according to the above-mentioned calculation method using the obtained measured values.
[0202] <Production of Powder Composition> [Example 1] A hydrated zirconia sol obtained by hydrolyzing an aqueous solution of zirconium oxychloride was mixed with yttria (Y2O3) so that the yttrium content was 2.5 mol%, and then dried. After that, it was heat-treated in an air atmosphere at 1160°C for 2 hours to obtain a calcined powder with a matrix of yttrium-containing zirconia (yttrium-stabilized zirconia) with an yttrium content of 2.5 mol%. The calcined powder obtained was mixed with pure water and pulverized in a ball mill using beads with a diameter of 2 mm as the milling medium for 18 hours to obtain a matrix of zirconia with an yttrium content of 2.5 mol% and a BET specific surface area of 11.9 m 2 A slurry containing a powder (yttrium-stabilized zirconia powder) having a molecular weight of 1 / g was obtained, and this was designated as Slurry A in Example 1.
[0203] A slurry with a BET specific surface area of 9.7 m was prepared by the same method as slurry A, except that yttrium was mixed so that the yttrium content was 5.5 mol% and milling was performed for 10 hours. A zirconia matrix with an yttrium content of 5.5 mol% (yttrium-stabilized zirconia) was used as the matrix. 2 / g, a slurry containing the powder was obtained. This was designated as Slurry B in Example 1. The BET specific surface area of the powder contained in Slurry A was 2.2 m 2 / gIt was big.
[0204] The slurry A was added to and mixed with the stirred slurry B so that the amount of yttrium in the powder composition was 4.5 mol %. The mixture was then dried at 110° C. under air flow to obtain a powder composition having a matrix of zirconia with an yttrium amount of 4.5 mol % (yttrium-stabilized zirconia) and a BET specific surface area of 10.4 m. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia powders contained in the powder composition (the stabilized zirconia powders contained in the two slurries) was 3.0 mol%.
[0205] [Example 2] Slurry A was added to and mixed with slurry B so that the amount of yttrium in the powder composition was 5.2 mol %. Except for this, a powder composition was prepared in the same manner as in Example 1, using zirconia with an yttrium amount of 5.2 mol % (yttrium-stabilized zirconia) as the matrix (main component) and having a BET specific surface area of 9.9 m. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0206] [Example 3] After drying the mixture of hydrated zirconia sol and yttria, the mixture was heat-treated in an air atmosphere at 1125°C for 6 hours, and the pulverization time in a ball mill was 8 hours. Except for this, a zirconia matrix containing 2.5 mol% yttrium (yttrium-stabilized zirconia) was used, and a BET specific surface area of 9.7 m was obtained by the same method as in Example 1. 2 / g, a slurry containing the powder was obtained. This was designated as Slurry A in Example 3. The BET specific surface area of the powder contained in Slurry A was equal to the BET specific surface area of the powder contained in Slurry B in Example 1.
[0207] Slurry A of Example 3 was added to and mixed with slurry B of Example 1 so that the amount of yttrium in the powder composition was 5.2 mol %. Other than that, a method similar to that of Example 1 was used to prepare a powder composition having a matrix of zirconia (yttrium-stabilized zirconia) with an yttrium amount of 5.2 mol % and a BET specific surface area of 9.7 m. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0208] [Example 4] After drying the mixture of hydrated zirconia sol and yttria, the mixture was heat-treated in an air atmosphere at 1045°C for 6 hours, and the pulverization time in a ball mill was set to 7 hours. Except for this, a zirconia matrix containing 2.5 mol% yttrium (yttrium-stabilized zirconia) was used, and a BET specific surface area of 14.4 m was obtained by the same method as in Example 1. 2 / g, a slurry containing the powder was obtained. This was designated as slurry A in Example 4. The BET specific surface area of the powder contained in slurry A was 4.7 m smaller than the BET specific surface area of the powder contained in slurry B in Example 1. 2 / gIt was big.
[0209] A powder composition having a BET specific surface area of 10.2 m2 and a matrix of zirconia (yttrium-stabilized zirconia) containing 5.2 mol% yttrium was prepared in the same manner as in Example 1, except that the slurry A of Example 4 was added to and mixed with the slurry B of Example 1 so that the amount of yttrium in the powder composition was 5.2 mol%. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0210] [Example 5] Slurry A was added to and mixed with slurry B so that the amount of yttrium in the powder composition was 5.4 mol%. Except for this, a powder composition was prepared in the same manner as in Example 1, using zirconia with an yttrium amount of 5.4 mol% as a matrix and a BET specific surface area of 9.8 m 2The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0211] [Example 6] The mixture of hydrated zirconia sol and yttria was dried and then heat-treated in an air atmosphere at 1145° C. Except for this, a zirconia matrix containing 5.5 mol % yttrium (yttrium-stabilized zirconia) was used, and a BET specific surface area of 10.8 m was obtained by the same method as in Example 1. 2 / g, a slurry containing the powder was obtained. This was designated as Slurry B in Example 6. Slurry A in Example 4 was used as Slurry A. The BET specific surface area of the powder contained in Slurry A was 3.6 m higher than the BET specific surface area of the powder contained in Slurry B. 2 / gIt was big.
[0212] A powder composition having a BET specific surface area of 11.2 m was prepared in the same manner as in Example 1, except that the slurry A of Example 4 was added to and mixed with the slurry B so that the yttrium content in the powder composition was 5.2 mol %. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0213] [Example 7] Yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 1.5 mol %. Other than that, a slurry having a BET specific surface area of 11.9 m2 was prepared by the same method as in slurry A of Example 1, using zirconia having an yttrium amount of 1.5 mol % as a matrix. 2 A slurry containing a powder (yttrium-stabilized zirconia powder) having a specific surface area of 0.1 μm / g was obtained. This was designated as slurry A of Example 7. Slurry B was the same as that of Example 1. The BET specific surface area of the powder contained in slurry A of Example 7 was 2.2 m2 smaller than the BET specific surface area of the powder contained in slurry B of Example 1. 2 / gIt was big.
[0214] A powder composition was prepared in the same manner as in Example 1, except that slurry A was added to and mixed with slurry B so that the amount of yttrium in the powder composition was 5.2 mol%. The powder composition was prepared using zirconia with an yttrium content of 5.2 mol% (yttrium-stabilized zirconia) as the matrix and had a BET specific surface area of 9.9 m. 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 4.0 mol %.
[0215] [Example 8] Yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 6.5 mol %. Other than that, a slurry having a BET specific surface area of 10.3 m2 was prepared by the same method as in the slurry B of Example 1, using zirconia having an yttrium amount of 6.5 mol % as a matrix. 2 A slurry containing a powder (yttrium-stabilized zirconia powder) having a specific surface area of 0.1 μm / g was obtained. This was designated as slurry B of Example 8. Slurry A of Example 1 was used as slurry A. The BET specific surface area of the powder contained in slurry A of Example 1 was 1.6 m less than the BET specific surface area of the powder contained in slurry B of Example 8. 2 / gIt was big.
[0216] The slurry A was added to and mixed with the slurry B so that the amount of yttrium in the powder composition was 5.2 mol%. Other than that, a powder composition was prepared in the same manner as in Example 1, using zirconia with an yttrium amount of 5.2 mol% as a matrix and a BET specific surface area of 10.8 m 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 4.0 mol %.
[0217] [Example 9] Using the slurry A and slurry B of Example 1, slurry A was added to slurry B under stirring so that the amount of yttrium in the powder composition was 5.0 mol % to obtain a mixed slurry. The mixed slurry was stirred at a stirring power of 0.5 kW / m 3The mixture was mixed at 40° C. for 0.5 hours and then dried. In this way, a mixture was prepared using zirconia with an yttrium content of 5.0 mol% (yttrium-stabilized zirconia) as the matrix and a BET specific surface area of 10.1 m 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0218] [Example 10] Using the slurry A and slurry B of Example 1, slurry A was added to slurry B under stirring so that the amount of yttrium in the powder composition was 5.0 mol % to obtain a mixed slurry. The mixed slurry was stirred at a stirring power of 0.01 kW / m 3 The mixture was mixed at 40° C. for 0.5 hours and then dried. In this way, a mixture was prepared using zirconia with an yttrium content of 5.0 mol% (yttrium-stabilized zirconia) as the matrix and a BET specific surface area of 10.1 m 2 The difference in the amount of stabilizing elements between the two stabilized zirconia particles contained in the powder composition was 3.0 mol %.
[0219] [Comparative Example 1] A hydrated zirconia sol obtained by hydrolyzing an aqueous solution of zirconium oxychloride was mixed with yttria so that the yttrium content was 2.5 mol%, and then dried. The obtained dried product was heat-treated at 1160°C for 2 hours in an air atmosphere to obtain a powder having a matrix of zirconia containing yttrium with an yttrium content of 2.5 mol%. The obtained powder was mixed with α-alumina and pure water. Mixing was performed for 8 hours by grinding and mixing using a ball mill with 2 mm beads as a grinding medium. As a result, a powder having a matrix of zirconia with an yttrium content of 2.5 mol%, containing 0.05 mass% alumina, and having a BET specific surface area of 10.0 m was obtained. 2 A slurry containing a powder (alumina-containing yttrium-stabilized zirconia powder) having a molecular weight of 1 / g was obtained. This was designated as slurry A in Comparative Example 1.
[0220] A slurry having a zirconia matrix containing 5.5 mol% yttrium, 0.05 mass% alumina, and a BET specific surface area of 10.0 m was prepared in the same manner as slurry A, except that the amount of yttrium in the yttrium-stabilized zirconia was set to 5.5 mol% and the grinding and mixing time in the ball mill was set to 10 hours. 2 / g, and this was designated as slurry B in Comparative Example 1. The BET specific surface area of the powder contained in slurry A was equal to the BET specific surface area of the powder contained in slurry B.
[0221] The slurry A and the slurry B were mixed so that the amount of yttrium in the powder composition was 4.0 mol %, and then dried. In this way, a powder composition having a zirconia matrix with an yttrium amount of 4.0 mol %, 0.05 mass % alumina, and a BET specific surface area of 10.0 m was obtained. 2 The difference in the amount of stabilizing elements in the stabilized zirconia contained in the powder composition was 3.0 mol%.
[0222] [Comparative Example 2] Yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 1.5 mol %, and heat treatment was performed at 1130° C. Other than that, a slurry was prepared in the same manner as slurry A in Comparative Example 1, in which zirconia having an yttrium amount of 1.5 mol % was used as a matrix, the alumina content was 0.05 mass %, and the BET specific surface area was 11.4 m 2 / g, a slurry containing the powder was obtained. This was designated as slurry A of Comparative Example 2. The BET specific surface area of the powder contained in this slurry A was 1.4 m2 larger than the BET specific surface area of the powder contained in slurry B of Comparative Example 1. 2 / gIt was big.
[0223] Except for using the obtained slurry A, the slurry A and the slurry B were mixed in the same manner as in Comparative Example 1. In this manner, a zirconia matrix containing 5.2 mol % yttrium, 0.05 mass % alumina, and a BET specific surface area of 10.1 m was obtained. 2The difference in the amount of stabilizing elements in the stabilized zirconia contained in the powder composition was 4.0 mol%.
[0224] [Comparative Example 3] A powder composition of Comparative Example 3 was obtained in the same manner as in Example 12 of JP 2021-059489 A. That is, yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 2.0 mol%, and α-alumina was not mixed. Other than this, a powder composition having a BET specific surface area of 10.2 m was obtained in the same manner as in the slurry A of Comparative Example 1, using zirconia with an yttrium amount of 2.0 mol% as the matrix. 2 / g, a slurry containing the powder was obtained. This was designated as slurry A of Comparative Example 3. The BET specific surface area of the powder contained in this slurry A was 2.2 m2 larger than the BET specific surface area of the powder contained in slurry B of Comparative Example 3. 2 / gIt was small.
[0225] A slurry was prepared in the same manner as slurry B of Comparative Example 1, except that yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 8.5 mol%, the heat treatment temperature was 1130°C, and α-alumina was not mixed. As a result, a slurry having a BET specific surface area of 12.4 m2 was prepared using zirconia with an yttrium amount of 8.5 mol% as a matrix. 2 This slurry was designated as Slurry B of Comparative Example 3.
[0226] The obtained slurries A and B were used. Except for this, a method similar to that of Comparative Example 1 was used to prepare a zirconia matrix having an yttrium content of 5.2 mol% and a BET specific surface area of 11.3 m. 2 The difference in the amount of stabilizing elements in the stabilized zirconia contained in the powder composition was 6.5 mol %.
[0227] [Comparative Example 4] A slurry having a BET specific surface area of 10.0 m2 and a zirconia matrix containing 5.5 mol% yttrium was prepared in the same manner as in the slurry B of Comparative Example 1.2 This slurry was designated as Slurry B of Comparative Example 4.
[0228] The obtained slurry B was dried to obtain a slurry having a matrix of zirconia containing 5.5 mol % yttrium, 0.05 mass % alumina, and a BET specific surface area of 10.0 m. 2 This was used as the powder (powder composition) of Comparative Example 4.
[0229] [Comparative Example 5] A slurry having a BET specific surface area of 10.0 m2 and a zirconia matrix containing 5.5 mol% yttrium was prepared in the same manner as in the slurry B of Comparative Example 1, except that α-alumina was not mixed. 2 This slurry was designated as Slurry B in Comparative Example 5.
[0230] The obtained slurry B was dried to obtain a slurry having a matrix of zirconia containing 5.5 mol% yttrium and a BET specific surface area of 10.0 m. 2 This was used as the powder (powder composition) of Comparative Example 5.
[0231] [Comparative Example 6] A slurry having a BET specific surface area of 11.3 m2 was prepared by the same method as in the slurry A of Comparative Example 1, except that α-alumina was not mixed and the calcination temperature was 1140°C. 2 This slurry was designated as Slurry A in Comparative Example 6.
[0232] A slurry was prepared in the same manner as slurry B of Comparative Example 1, except that yttria was mixed so that the amount of yttrium in the yttrium-stabilized zirconia was 7.5 mol % and that α-alumina was not mixed. As a result, a slurry having a BET specific surface area of 11.9 m2 was prepared using zirconia with an yttrium amount of 7.5 mol % as a matrix. 2 / g, a slurry containing the powder was obtained. This was designated as slurry B in Comparative Example 6. The BET specific surface area of the powder contained in slurry A was 0.6 m2 smaller than the BET specific surface area of the powder contained in slurry B. 2 / gIt was small.
[0233] A zirconia matrix having an yttrium content of 6.0 mol% and a BET specific surface area of 11.6 m was prepared in the same manner as in Comparative Example 1, except that the obtained slurries A and B were used and that the two slurries were mixed so that the yttrium content was 6.0 mol%. 2 / g, which was designated as the powder composition of Comparative Example 6. The difference in the amount of stabilizing elements in the stabilized zirconia contained in this powder composition was 5.0 mol%.
[0234] The amount of stabilizing elements (YO: mol%) in the powders contained in the slurries prepared in each Example and Comparative Example, and the difference in the amount of stabilizing elements (difference in YO) are shown in Table 1. The amount of stabilizing elements (mol% of YO), the content of added elements converted to oxide, and properties in the powder compositions obtained in each Example and Comparative Example are shown in Table 2.
[0235] [Table 1]
[0236] [Table 2]
[0237] In Examples 2 to 4 and 6 to 8, the amount of stabilizing elements (amount of yttrium) in the powder composition is the same. In Example 4, the BET specific surface area of the yttrium-containing zirconia, in which the amount of yttrium is 2.5 mol%, is high compared to Example 2, and the ΔV 1300 and ΔV 1500It can be confirmed that it is fast. Furthermore, for Example 2, Example 3 containing yttria-containing zirconia with a lower BET specific surface area and a yttria content of 2.5 mol% has a lower BET specific surface area of the obtained powder composition, but ΔV 1500 becomes faster compared to Example 2. From the comparison between Example 4 and Comparative Example 2, it can be confirmed that by containing alumina, ΔV 1300 becomes faster.
[0238] For Example 2, in Example 7, the yttrium content of the yttria-containing zirconia with a lower yttrium amount is lower. In this case, it can be confirmed that ΔV 1300 and ΔV 1500 are slower for Example 7 than for Example 2. For Example 2, in Example 8, the yttrium content of the yttria-containing zirconia with a higher yttrium amount is 6.5 mol%, which is higher than that of Example 2, and it can be confirmed that ΔV 1300 and ΔV 1500 are faster.
[0239] For Example 4, in Example 6, the BET specific surface area of the yttria-containing zirconia with a yttrium content of 5.5 mol% is high, and it can be confirmed that ΔV 1300 is fast and ΔV 1500 is slow for the powder composition.
[0240] <Measurement of the amount of stabilizing element by STEM-EDS> The amount of stabilizing element in the powder composition obtained in Example 2 was determined by STEM-EDS measurement (n = 1). Specifically, the composition of 10 non-overlapping powder particles was measured, and the frequency was determined when the data interval (class interval) of the amount of stabilizing element was 0.1 mol%. The measurement results were as shown in Fig. 3. The maximum value of the yttrium amount in the powder particles of yttria-containing zirconia was 6.5 mol%, and the minimum value was 2.7 mol%. Therefore, the difference (distribution width) between the maximum value and the minimum value of the yttrium amount was 3.8 mol%. From this, it was confirmed that the powder composition obtained in Example 2 contains two or more stabilized zirconias with different amounts of stabilizing elements.
[0241] The STEM-EDS measurement of the powder composition obtained in Example 2 was carried out two more times (n=2, n=3). Each measurement was carried out using different powder particles. These measurements were carried out in the same manner as in the case of n=1.
[0242] The distribution width of the yttrium amount (difference between the maximum value and the minimum value) was 3.8 mol% when n=1, 4.4 mol% when n=2, and 3.7 mol% when n=3. From these results, it was confirmed that the powder composition of Example 2 had a sufficiently small variation in distribution width. Therefore, it was confirmed that in the powder composition of Example 2, stabilized zirconia particles having different yttrium amounts were dispersed with high uniformity.
[0243] The powder composition obtained in Comparative Example 5 was subjected to STEM-EDS measurement in the same manner as the powder composition in Example 2 (only n=1). As a result, the maximum value of the yttrium content of the zirconia powder particles was 6.4 mol%, and the minimum value was 4.9 mol%. Thus, the difference between the maximum and minimum values of the yttrium content (distribution width) was 1.5 mol%. Since the difference in Y2O3 in Comparative Example 5 shown in Table 1 was also 0 mol%, it was confirmed that the powder composition obtained in Comparative Example 5 did not contain two or more stabilized zirconias with different amounts of stabilizing elements.
[0244] <Production of calcined body> [Examples 11 to 17, Comparative Examples 7 and 9] The powder compositions obtained in the same manner as in Examples 2 and 5 to 10, and Comparative Examples 2, 3, and 5 were filled into a die having a diameter of 25 mm, and were subjected to uniaxial press molding at a pressure of 49 MPa and CIP treatment at a pressure of 196 MPa to obtain a molded body. The obtained molded body was calcined in an air atmosphere at a calcination temperature of 1000°C for 1 hour to obtain the calcined bodies of Examples 11 to 17 and Comparative Examples 7 to 9. The powder compositions used in each Example and Comparative Example and the properties of the calcined bodies are shown in Table 3.
[0245] [Table 3]
[0246] The ΔV of Example 2 1300 is 0.058% / °C -1 and the ΔV of Example 11 1300 is 0.060% / °C -1 From this, it can be confirmed that the powder composition and the calcined body obtained by calcining the powder composition have equivalent ΔV 1300 It can be confirmed that the calcined body of Example 11 has a T + C phase ratio of 100%. From this, it can be confirmed that the T + C phase ratio becomes higher by heat treatment compared to the powder composition. Examples 12 to 17 and Examples 5 to 10 which are precursors have equivalent ΔV 1300 It can be confirmed that they have. It can be confirmed that the calcined bodies of Examples 13 to 17 have a T + C phase ratio of 100%.
[0247] It can be confirmed that the calcined body of each example has a Vickers hardness suitable for shape processing such as CAM processing.
[0248] <Measurement of the amount of stabilizing element (yttrium amount) by STEM - EDS> The calcined body obtained in Example 11 was dry - pulverized in a mortar, and in the same manner as the powder composition of Example 2, the amount of yttrium in the calcined body was measured by STEM - EDS measurement. The measurement results were as shown in Fig. 4. The maximum value of the amount of yttrium in the powder particles of stabilized zirconia was 6.2 mol%, and the minimum value was 2.9 mol%. Therefore, the difference (distribution width) between the maximum value and the minimum value of the amount of yttrium was 3.3 mol%. From this, it was confirmed that the calcined body obtained in Example 11 contains two or more stabilized zirconias with different amounts of stabilizing elements.
[0249] The amount of yttrium in the calcined body obtained in Comparative Example 9 was measured in the same manner as in Example 11. The measurement results are shown in FIG. 5. The maximum amount of yttrium in the powder particles of stabilized zirconia was 6.5 mol%, and the minimum amount was 5.0 mol%. Therefore, the difference between the maximum and minimum amounts of yttrium (distribution width) was 1.5 mol%. Since the difference in Y2O3 in Comparative Example 5 shown in Table 1 was also 0 mol%, it was confirmed that the calcined body obtained in Comparative Example 9 did not contain two or more stabilized zirconias with different amounts of stabilizing elements.
[0250] <Production of sintered body> [Examples 18 to 27 and Comparative Examples 10 to 15] The powder compositions obtained in Examples 1 to 10, and the powder compositions and powders obtained in Comparative Examples 1 to 6 were each filled into a mold having a diameter of 25 mm, and molded by uniaxial press molding at a pressure of 49 MPa and CIP treatment at a pressure of 196 MPa to obtain a molded body.
[0251] The obtained compacts were calcined in an air atmosphere at a calcination temperature of 1000°C for 1 hour to obtain calcined bodies. The obtained calcined bodies were heated in an air atmosphere from room temperature to 1050°C at a heating rate of 250°C / min, and from 1050°C to 1580°C at a heating rate of 50°C / min. After heating, the sintering temperature was kept at 1580°C for 8 minutes, and then cooled to 900°C at a rate of 60°C / min. The sintered bodies were then removed from the sintering furnace (hereinafter also referred to as "short-time sintering program") to obtain sintered bodies of Examples 18 to 27 and Comparative Examples 10 to 15 (hereinafter also referred to as "short-time sintered bodies").
[0252] In addition, the calcined body obtained by the same procedure was sintered for 2 hours in an air atmosphere at a heating rate of 600°C / hour and a sintering temperature of 1500°C to obtain a sintered body (hereinafter also referred to as a "normal sintered body"). The ratio of the light transmittance of the short-time sintered body to the light transmittance of the normal sintered body thus obtained (light transmittance ratio) [%] was calculated. The results are shown in Table 4.
[0253] [Table 4]
[0254] It can be seen that the ordinary sintered body of Comparative Example 10 had a low light transmittance, but all the other ordinary sintered bodies had a light transmittance exceeding 45%.
[0255] The light transmittance of the sintered bodies (short-time sintered bodies) of each Example exceeded 45%, confirming that they had translucency suitable for use as a front tooth denture. On the other hand, the light transmittance of the sintered bodies (short-time sintered bodies) of each Comparative Example was 45% or less, and did not have the translucency required for a front tooth denture.
[0256] Comparative Example 10, in which the amount of yttrium is 4.0 mol%, has a ΔV 1300 0.07%℃ -1 It was confirmed that the light transmittance did not change between the normal sintered body and the short-time sintered body, even though the time exceeded 100 s. However, in Comparative Example 10, the light transmittance was 45% or less even in the normal sintered body, and it did not have a light transmittance suitable for use as a front denture.
[0257] ΔV 1300 0.07%℃ -1 It can be confirmed that the short-time sintered body of Comparative Example 11 obtained from the powder composition of Comparative Example 2 exceeding 100 nm has significantly reduced translucency compared to the normal sintered body, and does not have translucency sufficient for use as a front tooth denture.
[0258] The powder composition of Comparative Example 3 containing stabilized zirconia with an yttrium content of more than 8.0 mol%, the powder of Comparative Example 5 not containing two or more stabilized zirconias with different stabilizing element contents, and the powder composition of Comparative Example 6 containing a stabilizing element content (yttrium content) of 5.8 mol% or more, have a ΔV 1300 0.07%℃ -1 Nevertheless, in Comparative Examples 12, 14, and 15 using these powder compositions, the translucency of the short-time sintered body was significantly lower than that of the normal sintered body. Therefore, it was confirmed that the translucency suitable for use as a front denture was not obtained.
[0259] Table 5 shows the evaluation results of the short-time sintered compacts obtained in Examples 19 to 27 and Comparative Examples 10 to 14.
[0260] [Table 5]
[0261] The average crystal grain size of the sintered bodies of each Example shown in Table 5 was 2.5 μm or less, and the crystal grain size difference was also small. All of these were sintered bodies with a matrix of stabilized zirconia with a tetragonal prime phase as the main phase. In other words, it can be confirmed that they are sintered bodies of stabilized zirconia whose crystal phase is tetragonal prime phase. The sintered body of Example 19 had a biaxial bending strength of 745 MPa. It was confirmed that the crystal grain size difference of the sintered bodies of each Example was 0.10 μm or less. It was confirmed that the sintered bodies of Examples 21 to 26 have a biaxial bending strength of 800 MPa or more, and therefore can be applied to a connected bridge of four or more teeth based on JIS T 6526.
[0262] The Weibull coefficient of the sintered body of Example 26 was 8.0, and the Weibull coefficient of the sintered body of Example 27 was 3.2. Thus, the sintered body of Example 26, in which the stirring power required for preparing the powder composition was within a preferred range, was able to have a higher Weibull coefficient than the sintered body of Example 27.
[0263] The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2021-150878, filed on September 16, 2021, are hereby incorporated by reference as the disclosure of the specification of the present disclosure.
Claims
1. The matrix contains stabilized zirconia containing a stabilizing element, The sintered body is characterized in that the content of the stabilizing element is more than 4.0 mol% and not more than 5.8 mol%, the average crystal grain size is 2.5 μm or less, the crystal grain size difference is 0.10 μm or less, and further, the tetragonal prime phase fraction is 70% or more, the light transmittance is more than 45%, and the biaxial bending strength is 650 MPa or more.
2. 2. The sintered body according to claim 1, wherein the stabilizing element is one or more selected from the group consisting of yttrium, calcium and magnesium.
3. 3. The sintered body according to claim 1, which does not contain any undissolved stabilizing element.
4. 3. The sintered body according to claim 1, which has a matrix of stabilized zirconia having a tetragonal prime phase as a main phase.
5. 3. The sintered body according to claim 1, having a Weibull coefficient of 4.0 or more.
6. A calcined body containing two or more stabilized zirconias having different contents of stabilizing elements, the content of the stabilizing elements in the calcined body being more than 4.0 mol% and not more than 5.8 mol%, and the rate of change in thermal shrinkage rate per unit temperature at 1300°C is 0.07%°C or less. -1 The rate of change in the thermal shrinkage rate per unit temperature at 1500°C is 0.02%°C or less. -1 The method for producing a sintered body further comprises a step of sintering the calcined body under the following conditions, the calcined body being characterized in that the content of the stabilizing element in each of two or more stabilized zirconias different from each other is 8.0 mol% or less. Sintering method: normal pressure sintering Sintering atmosphere: Oxidizing atmosphere Sintering temperature: 1450°C or higher and 1650°C or lower Sintering time: 3 minutes to 30 minutes Heating rate: (room temperature to 1050°C) 150° C. / min or more and 350° C. / min or less (1050°C to sintering temperature) 30° C. / min or more and 150° C. / min or less Temperature drop rate: (from sintering temperature to 900°C) 30° C. / min or more and 300° C. / min or less
7. A dental prosthetic material comprising the sintered body according to claim 1 or 2.
8. A denture for anterior teeth, comprising the sintered body according to claim 1 or 2.
Citation Information
Patent Citations
Translucent yttria-containing zirconia sintered compact, manufacturing method and utilization of the same
JP2008222450A
Sintered body of zirconia and method for manufacturing the same
JP2011073907A
Zirconia sintered body, and manufacturing method thereof
JP2014218421A
Zirconia sintered body and production method thereof
JP2021059489A
Light-transmitting zirconia sintered compact, zirconia powder and application thereof
JP2015143178A