Liquid crystal alignment agent, liquid crystal alignment film and liquid crystal display
A liquid crystal aligning agent with specific polyimide precursors and imidized polymers enhances liquid crystal orientation and contrast in display elements by addressing in-plane brightness variations and alignment issues.
Patent Information
- Application Number
- JP2024139706
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-07-17
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing liquid crystal display elements suffer from in-plane brightness variations during black display due to manufacturing variations, leading to reduced contrast and alignment issues in photoalignment methods compared to conventional rubbing treatment.
A liquid crystal aligning agent containing specific polyimide precursors with repeating units and imidized polymers, incorporating amide or urea bonds for enhanced hydrogen bonding, and a naphthalene skeleton for improved heat resistance and alignment properties, is used to form a liquid crystal alignment film.
The solution provides a liquid crystal display element with high liquid crystal orientation and suppressed in-plane brightness variation, resulting in improved contrast and stability.
Smart Images

Figure 2024161565000001 
Figure 2024161565000002 
Figure 2024161565000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film, and a liquid crystal display element. [Background technology]
[0002] Conventionally, liquid crystal display devices have been widely used as display units for personal computers, smartphones, mobile phones, televisions, etc. A liquid crystal display device usually includes a liquid crystal layer sandwiched between an element substrate and a color filter substrate, pixel electrodes and a common electrode for applying an electric field to the liquid crystal layer, an alignment film for controlling the alignment of liquid crystal molecules in the liquid crystal layer, and thin film transistors (TFTs) for switching electric signals supplied to the pixel electrodes. Known methods for driving liquid crystal molecules include vertical electric field methods such as the TN method and the VA method, and horizontal electric field methods such as the IPS (In Plane Switching) method and the FFS (Fringe Field Switching) method.
[0003] The most industrially widespread liquid crystal alignment film is prepared by rubbing the surface of a film made of polyamic acid and / or polyimide obtained by imidizing the polyamic acid formed on an electrode substrate in one direction with a cloth such as cotton, nylon, or polyester, which is called a rubbing treatment. The rubbing treatment is an industrially useful method that is simple and has excellent productivity. However, with the increase in performance, definition, and size of liquid crystal display elements, various problems have become clear, such as scratches on the surface of the alignment film caused by the rubbing treatment, dust generation, effects due to mechanical force and static electricity, and even non-uniformity within the alignment treatment surface. As an alignment treatment method that replaces the rubbing treatment, a photoalignment method is known in which liquid crystal alignment ability is imparted by irradiating polarized radiation. As for the photoalignment method, methods utilizing photoisomerization reaction, photocrosslinking reaction, photodecomposition reaction, and the like have been proposed (see Non-Patent Document 1, Patent Documents 1 and 2).
[0004] A liquid crystal alignment film, which is a component of a liquid crystal display element, is a film for uniformly aligning liquid crystals, and liquid crystal alignment is one of its important characteristics. However, the liquid crystal alignment film obtained by the above-mentioned photoalignment method tends to have lower liquid crystal alignment properties than the liquid crystal alignment film obtained by the conventional rubbing treatment, and the range of application of liquid crystal display devices equipped with the liquid crystal alignment film has been limited. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 9-297313 [Patent Document 2] International Publication No. 2015 / 050135 Brochure [Non-patent literature]
[0006] [Non-Patent Document 1] "Functional Materials" November 1997 Vol. 17, No. 11, pages 13-22 Summary of the Invention [Problem to be solved by the invention]
[0007] Furthermore, in actual liquid crystal display elements, the twist angle varies slightly within the plane of the liquid crystal display element due to manufacturing variations, etc. This in-plane variation causes the brightness of the liquid crystal display element when displaying black to vary within the plane. The present invention has been made in consideration of the above circumstances, and has as its object to provide a liquid crystal alignment agent that can provide a liquid crystal display element having high liquid crystal alignment properties, suppressing in-plane brightness variations during black display, and improving contrast. [Means for solving the problem]
[0008] The present inventors have conducted extensive research and found that the above problems can be solved by using a liquid crystal aligning agent containing a specific component, and have completed the present invention.
[0009] A liquid crystal aligning agent comprising at least one polymer (A) selected from the group consisting of a polyimide precursor having a repeating unit (a1) represented by the following formula (1) and a repeating unit (a2) represented by the following formula (2), and an imidized polymer thereof:
[0010] [ka] (In the formula, R1 to R4 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms containing a fluorine atom, or a phenyl group, and at least one of R1 to R4 represents a group other than a hydrogen atom as defined above. R and Z each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Y1 represents a divalent organic group represented by the following formula (H).)
[0011] [ka] (Q1 represents a divalent organic group having 1 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1. * represents a bond. *1 represents a bond bonded to a carbon atom.)
[0012] [ka] (In the formula, R1 to R4, R, and Z are defined as in the above formula (1). Y2 represents a divalent organic group represented by the following formula (O).)
[0013] [ka] (Each Ar independently represents a benzene ring, a biphenyl structure, or a naphthalene ring, and at least one of the two Ar represents a naphthalene ring. Any hydrogen atom on the ring may be replaced with a halogen atom or a monovalent organic group. Q2 is -(CH2) n -(n is an integer of 2 to 18), or the above -(CH2) n represents a group in which a portion of - is replaced with -O-, -C(=O)-, or -OC(=O)-. * represents a bond. In this specification, when it is obvious that the term is an integer, such as "n is an integer of 2 to 18", the "integer" may be omitted. In addition, in all cases, * represents a bond. Boc represents a tert-butoxycarbonyl group. Fmoc represents a 9-fluorenylmethyloxycarbonyl group. Effect of the Invention
[0014] According to the present invention, there are provided a liquid crystal display element having high liquid crystal alignment properties and excellent contrast in which in-plane brightness variations during black display are suppressed, and a liquid crystal aligning agent capable of obtaining the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Polymer (A)> The liquid crystal alignment agent of the present invention contains at least one polymer (A) selected from the group consisting of polyimide precursors having a repeating unit (a1) represented by the following formula (1) and a repeating unit (a2) represented by the following formula (2) and imidized polymers thereof. The polymer (A) may be composed of one or more types. The polymer (A) contains the repeating unit (a1) or an imidized structural unit of the repeating unit (a1), and thus has an amide bond or urea bond having hydrogen bonding properties in the molecule, and thus the heat resistance of the resulting liquid crystal alignment film is increased, and a decrease in contrast due to variations in the twist angle in the plane of the liquid crystal display element generated during production is suppressed. In addition, by further containing the repeating unit (a2) or an imidized structural unit of the repeating unit (a2), the polymer has a naphthalene skeleton having excellent heat resistance and liquid crystal alignment properties in the molecule, and thus the heat resistance and liquid crystal alignment properties of the resulting liquid crystal alignment film are increased, and a liquid crystal display element having excellent contrast can be obtained. Due to the above synergistic effect, a liquid crystal display element having high liquid crystal alignment properties and excellent contrast can be obtained from the liquid crystal alignment agent of the present invention.
[0016] [ka] (In the formula, R1 to R4 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms containing a fluorine atom, or a phenyl group, and at least one of R1 to R4 represents a group other than a hydrogen atom as defined above. R and Z each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Y1 represents a divalent organic group represented by the following formula (H).)
[0017] [ka] (Q1 represents a divalent organic group having 1 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1. *1 represents a bond bonded to a carbon atom.)
[0018] [ka] (In the formula, R1 to R4, R, and Z are defined as in the above formula (1). Y2 represents a divalent organic group represented by the following formula (O).)
[0019] [ka] (Each Ar independently represents a benzene ring, a biphenyl structure, or a naphthalene ring, and at least one of the two Ar represents a naphthalene ring. Any hydrogen atom on the ring may be replaced with a halogen atom or a monovalent organic group. Q2 is -(CH2) n -(n is an integer of 2 to 18), or the above -(CH2) n represents a group in which a portion of - is replaced with -O-, -C(=O)-, or -OC(=O)-.
[0020] Specific examples of the alkyl group having 1 to 6 carbon atoms in R1 to R4 include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and an n-pentyl group. Specific examples of the alkenyl group having 2 to 6 carbon atoms in R1 to R4 include a vinyl group, a propenyl group, and a butynyl group, which may be linear or branched. Specific examples of the alkynyl group having 2 to 6 carbon atoms in R1 to R4 include an ethynyl group, a 1-propynyl group, and a 2-propynyl group. Examples of the halogen atom in R1 to R4 include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the monovalent organic group having 1 to 6 carbon atoms and containing a fluorine atom in R1 to R4 include a fluoromethyl group and a trifluoromethyl group. From the viewpoint of high photoreactivity, R1 to R4 are hydrogen atoms or methyl groups, preferably at least one of R1 to R4 is a methyl group, more preferably at least two of R1 to R4 are methyl groups, and even more preferably, R1 and R3 are methyl groups, and R2 and R4 are hydrogen atoms. In order to obtain the effects of the present invention satisfactorily, at least one of R1 to R4 represents a group other than a hydrogen atom as defined above. The above-mentioned configuration increases the photoreactivity of the polyimide film and increases the in-plane anisotropy of the resulting liquid crystal alignment film, thereby suppressing the decrease in contrast caused by the variation in twist angle within the liquid crystal display element plane that occurs during production.
[0021] Q1 in the above formula (H) represents a divalent organic group having 1 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1, and among them, -NH-C(=O)-, -NH-C(=O)-NH-, or a divalent organic group having 2 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1 is preferred. *1 is defined as in the above formula (H). Specific examples of the divalent organic group having 2 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1 include a divalent organic group (a1) having 2 to 18 carbon atoms in which a part of the -CH2- in the alkylene group having 2 to 18 carbon atoms is replaced with either *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1, and a divalent organic group (a2) having 2 to 18 carbon atoms in which a part of the -CH2- in the divalent organic group (a1) is replaced with at least one group selected from the group consisting of -O-, -C(=O)O-, -C=C-, -C≡C-, a cyclohexylene group, and a phenylene group. Among these, from the viewpoint of obtaining the effects of the present invention satisfactorily, the above divalent organic group (a1) or a group in which part of the -CH2- in the above divalent organic group (a1) is replaced with -O- is preferred.
[0022] As the divalent organic group represented by the above formula (H), a divalent organic group represented by any one of the following formulae (h-1) to (h-6) is preferred, from the viewpoint of obtaining the effects of the present invention satisfactorily.
[0023] [ka]
[0024] Any hydrogen atom on the ring of Ar in the above formula (O) may be replaced with a halogen atom or a monovalent organic group such as an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group containing a fluorine atom having 1 to 6 carbon atoms, etc. Specific examples of these monovalent organic groups include the structures exemplified for R1 to R4 above. As specific examples of the divalent organic group represented by the above formula (O), divalent organic groups represented by any of the following formulae (o-1) to (o-6) are preferred from the viewpoint of improving liquid crystal alignment properties.
[0025] [ka]
[0026] From the viewpoint of obtaining the effects of the present invention satisfactorily, the above polymer (A) may further be at least one polymer selected from the group consisting of a polyimide precursor having a repeating unit (a2') represented by the following formula (2') and an imidized polymer thereof: [ka] (X 2’ represents a tetravalent organic group, Y 2’ represents a divalent organic group represented by the following formula (O2). R and Z are the same as those in the above formula (1). [ka] (Ar 2’ represents a benzene ring, and any hydrogen atom on the ring may be replaced by a halogen atom or a monovalent organic group. 2’ is a single bond, -O-, -C(=O)-, -OC(=O)-, -(CH2) n -(n is 2 to 18), or the above -(CH2) n represents a group in which a part of - is replaced with -O-, -C(=O)- or -OC(=O)-. m is an integer of 0 to 2. 2’ , Q 2’ When multiple are present, they may be the same or different.)
[0027] X 2’ Examples of the tetravalent organic group include a tetravalent organic group represented by the following formula (g), a tetravalent organic group represented by any one of the following formulas (X-1) to (X-25), and a tetravalent organic group derived from an aromatic tetracarboxylic dianhydride.
[0028] [ka] (R1, R2, R3, and R4 are defined as R1, R2, R3, and R4 in the above formula (1).)
[0029] [ka] [ka]
[0030] Here, the aromatic tetracarboxylic dianhydride refers to an acid dianhydride obtained by intramolecular dehydration of a carboxy group bonded to an aromatic ring such as a benzene ring or a naphthalene ring. Specific examples include tetravalent organic groups represented by any of the following formulae (Xa-1) to (Xa-2) and tetravalent organic groups represented by any of the following formulae (Xr-1) to (Xr-7).
[0031] [ka] (x and y each independently represent a single bond, an ether, a carbonyl, an ester, an alkanediyl group having 1 to 10 carbon atoms, 1,4-phenylene, a sulfonyl, or an amido group. j and k are 0 or 1.)
[0032] [ka]
[0033] The tetravalent organic group represented by the above formula (Xa-1) or (Xa-2) may have a structure represented by any one of the following formulas (Xa-3) to (Xa-19).
[0034] [ka]
[0035] [ka]
[0036] Ar in the above formula (O2) 2’ Any hydrogen atom on the ring may be replaced with a monovalent organic group such as a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms and containing a fluorine atom, etc. Specific examples of these monovalent organic groups include the structures exemplified for R1 to R4 above. As the divalent organic group represented by the above formula (O2), a divalent organic group represented by any one of the following formulae (o2-1) to (o2-11) is preferred from the viewpoint of reducing the occurrence of AC afterimages.
[0037] [ka]
[0038] From the viewpoint of improving adhesion to a sealing agent and voltage retention characteristics, the above polymer (A) may further be at least one polymer selected from the group consisting of polyimide precursors having a repeating unit (a3) represented by the following formula (3) and imidized polymers thereof:
[0039] [ka] (In the formula, R and Z are the same as those in the formula (1). X3 represents a tetravalent organic group, and Y3 represents a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate protecting group)" in the molecule.)
[0040] Specific examples of X3 include the above X 2’In order to satisfactorily obtain the effects of the present invention, X3 is preferably a tetravalent organic group represented by the above formula (g) or a tetravalent organic group represented by any one of the above formulas (X-1) to (X-25), and more preferably a tetravalent organic group represented by the above formula (g).
[0041] Specific examples of the divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate-based protecting group)" in the molecule in Y3 include a divalent organic group having a partial structure represented by the following formula (3-1) or a divalent organic group represented by the following formula (3-2).
[0042] [ka]
[0043] In the formula, Q5 is a single bond, -(CH2) n -(n is 1 to 20), or the -(CH n Any -CH2- in - is -O-, -COO-, -OCO-, -NQ9-, -NQ9CO-, -CONQ9-, -NQ9-CO-NQ 10 -, -NQ9-COO- or -O-COO-; 10 each independently represents a hydrogen atom or a monovalent organic group. Q6 and Q7 each independently represent -H, -NHD, -N(D)2, a group having -NHD, or a group having -N(D)2. Q8 represents -NHD, -N(D)2, a group having -NHD, or a group having -N(D)2. D represents a carbamate-based protecting group, and examples of the carbamate-based protecting group include a tert-butoxycarbonyl group or a 9-fluorenylmethoxycarbonyl group. However, at least one of Q5, Q6, and Q7 has a carbamate-based protecting group in the group.
[0044] From the viewpoint of reducing AC afterimages, preferred specific examples of Y3 include divalent organic groups represented by any of the following formulas (Y3-1) to (Y3-5).
[0045] [ka]
[0046] The polymer (A) may be at least one polymer selected from the group consisting of polyimide precursors having a repeating unit (a4) represented by the following formula (4) in addition to the repeating unit (a1), repeating unit (a2), repeating unit (a2') and repeating unit (a3) and imidized polymers thereof:
[0047] [ka]
[0048] In the formula, X4 represents a tetravalent organic group, and Y4 represents a divalent organic group. R and Z are the same as R and Z in the above formula (1), respectively. However, Y4 represents a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate-based protecting group)" in the molecule, or a structure other than the divalent organic group represented by the above formula (O2), and when X4 is the same as the tetravalent organic group represented by the above formula (g), Y4 represents a structure other than the divalent organic group represented by the above formula (H) or the divalent organic group represented by the above formula (O). Specific examples of X4 include the structures exemplified for X3.
[0049] Specific examples of X4 include the above X 2’ In order to satisfactorily obtain the effects of the present invention, X4 is preferably a tetravalent organic group represented by the above formula (g) or a tetravalent organic group represented by any one of the above formulas (X-1) to (X-25), and more preferably a tetravalent organic group represented by the above formula (g).
[0050] Specific examples of the divalent organic group of Y4 include a divalent organic group represented by the above formula (H), a divalent organic group represented by the above formula (O), a divalent organic group represented by the above formula (O2), or a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate protecting group)" in the molecule, a divalent organic group represented by any of the following formulas (g-1) to (g-5), and a divalent organic group derived from a diamine described below (a divalent organic group obtained by removing two amino groups from a diamine). Diamines having at least one nitrogen atom-containing structure selected from the group consisting of a nitrogen atom-containing heterocycle, a secondary amino group, and a tertiary amino group (hereinafter also referred to as a nitrogen atom-containing structure. However, in the above secondary amino group and tertiary amino group, the amino group is not bonded to a carbamate-based protecting group), 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, 2,4- Diaminobenzoic acid, 2,5-diaminobenzoic acid or 3,5-diaminobenzoic acid, diamines having a carboxy group such as the diamine compounds represented by the following formulae (3b-1) to (3b-4), 4-(2-(methylamino)ethyl)aniline, 4-(2-aminoethyl)aniline, 4,4'-diaminobenzophenone, 1-(4-aminophenyl)-1,3,3-trimethyl-1H-indan-5-amine, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl- Diamines having a photopolymerizable group at the end, such as 1H-inden-6-amine, 2-(2,4-diaminophenoxy)ethyl methacrylate, 2,4-diamino-N,N-diallylaniline, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, cholestanyl 3,5-diaminobenzoate, cholestanyl 3,5-diaminobenzoate, lanostannyl 3,5-diaminobenzoate, 3,6-bis Diamines having a steroid skeleton, such as (4-aminobenzoyloxy)cholestane; diamines represented by any one of the following formulas (V-1) to (V-6); diamines having a siloxane bond, such as 1,3-bis(3-aminopropyl)-tetramethyldisiloxane; diamines having an oxazoline ring structure, such as those represented by the following formulas (Ox-1) to (Ox-2), and other divalent organic groups derived from diamines; and groups represented by any one of the formulas (Y-1) to (Y-167) described in WO 2018 / 117239.
[0051] [ka] [ka] (In (3b-1) above, A 1 represents a single bond, -CH2-, -C2H4-, -C(CH3)2-, -CF2-, -C(CF3)2-, -O-, -CO-, -NH-, -N(CH3)-, -CONH-, -NHCO-, -CHO-, -OCH2-, -COO-, -OCO-, -CON(CH3)- or -N(CH3)CO-, m1 and m2 each independently represent an integer of 0 to 4, and m1+m2 represents an integer of 1 to 4. In formula (3b-2), m3 and m4 each independently represent an integer of 1 to 5. In formula (3b-3), A 2 represents a linear or branched alkyl group having 1 to 5 carbon atoms, and m5 is 1 to 5. 3 and A 4 each independently represents a single bond, -CH2-, -C2H4-, -C(CH3)2-, -CF2-, -C(CF3)2-, -O-, -CO-, -NH-, -N(CH3)-, -CONH-, -NHCO-, -CHO-, -OCH2-, -COO-, -OCO-, -CO-N(CH3)- or -N(CH3)-CO-, and m6 is an integer of 1 to 4.
[0052] [ka]
[0053] (In the above formulas (V-1) to (V-6), X v1 ~X v4 , X p1 ~X p2 are each independently -(CH2) a - (a is 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -CH2-OCO-, -COO-, or -OCO-; X v5 represents -O-, -CH2O-, -CH2OCO-, -COO-, or -OCO-. Xa represents a single bond, -O-, -NH-, -O-(CH2) m -O- (m is 1 to 6), R v1 ~R v4 , R 1a ~R 1beach independently represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms.
[0054] [ka]
[0055] Examples of the nitrogen atom-containing heterocycle include pyrrole, imidazole, pyrazole, triazole, pyridine, pyrimidine, pyridazine, pyrazine, indole, benzimidazole, purine, quinoline, isoquinoline, naphthyridine, quinoxaline, phthalazine, triazine, carbazole, acridine, piperidine, piperazine, pyrrolidine, hexamethyleneimine, etc. Among these, pyridine, pyrimidine, pyrazine, piperidine, piperazine, quinoline, carbazole, or acridine is preferred.
[0056] The secondary amino group and tertiary amino group that the diamine having a nitrogen atom-containing structure may have are represented, for example, by the following formula (n). [ka]
[0057] In the above formula (n), R represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. "*1" represents a bond bonded to the hydrocarbon group. Examples of the monovalent hydrocarbon group R in the above formula (n) include alkyl groups such as methyl, ethyl, and propyl groups; cycloalkyl groups such as cyclohexyl groups; and aryl groups such as phenyl and methylphenyl groups. R is preferably a hydrogen atom or a methyl group.
[0058] Specific examples of diamines having a nitrogen atom-containing structure include 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, 1,4-bis-(4-aminophenyl)-piperazine, 3,6-diaminoacridine, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine, 4,4'-diaminodiphenylamine, N,N-bis(4-aminophenyl)-methylamine, or compounds represented by any of the following formulae (z-1) to (z-28).
[0059] [ka] [ka] [ka] (In the formula, Py represents a pyridine ring or a pyrimidine ring.)
[0060] From the viewpoint of obtaining the effects of the present invention well, the polymer (A) preferably has a repeating unit (a1) and the imidized structural unit of the repeating unit (a1) in total of 1 to 40 mol %, more preferably 1 to 35 mol %, and even more preferably 1 to 30 mol % of all repeating units. The total here includes a case where either the repeating unit (a1) or the imidized structural unit of the repeating unit (a1) is 0 mol %. Hereinafter, the total also includes a case where one or more of the structural unit elements are 0 mol %.
[0061] From the viewpoint of obtaining the effects of the present invention satisfactorily, the polymer (A) preferably contains the repeating unit (a1), the repeating unit (a2) and their imidized structural units in an amount of 5 mol % or more, and more preferably 10 mol % or more, of the total repeating units.
[0062] From the viewpoint of obtaining the effects of the present invention satisfactorily, in the polymer (A), the sum of the repeating unit (a2) and the imidized structural units of the repeating unit (a2) is preferably 1 to 95 mol %, more preferably 1 to 90 mol %, and even more preferably 5 to 90 mol %, of all repeating units.
[0063] From the viewpoint of obtaining the effects of the present invention satisfactorily, the sum of the repeating unit (a3) and the imidized structural units of the repeating unit (a3) in the polymer (A) is preferably 1 to 40 mol %, more preferably 1 to 30 mol %, and even more preferably 1 to 25 mol %, of all repeating units.
[0064] <Polymer (B)> The liquid crystal aligning agent of the present invention may contain, in addition to the polymer (A), a polymer (B) that does not have both the repeating unit (a1) and the repeating unit (a2) in the same molecule. The polymer (B) may be composed of one type or two or more types. From the viewpoint of obtaining the effects of the present invention well, examples of the polymer (B) include a polymer having at least one repeating unit selected from the group consisting of the repeating unit (b1) represented by the following formula (5) and the imidized structural unit of the repeating unit (b1). The repeating units constituting the polymer (B) may be composed of one type or two or more types. [ka] (In the formula, X5 is a tetravalent organic group, and Y5 is a divalent organic group. Each Z independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group. R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.)
[0065] The tetravalent organic group in the formula X5 may be a tetravalent organic group derived from an aliphatic tetracarboxylic dianhydride, a tetravalent organic group derived from an alicyclic tetracarboxylic dianhydride, or a tetravalent organic group derived from an aromatic tetracarboxylic dianhydride, and specific examples include the tetravalent organic groups exemplified for the above X4. From the viewpoint of obtaining the effects of the present invention well, X5 is preferably a tetravalent organic group represented by the above formula (g), a tetravalent organic group represented by any one of the above formulas (X-1) to (X-25), a tetravalent organic group represented by any one of the above formulas (Xa-1) to (Xa-2), or a tetravalent organic group represented by any one of the above formulas (Xr-1) to (Xr-7) (collectively referred to as a specific tetravalent organic group).
[0066] In order to satisfactorily obtain the effects of the present invention, the polymer (B) preferably contains repeating units in which X5 is the specific tetravalent organic group in an amount of 5 mol % or more, and more preferably 10 mol % or more, of all repeating units contained in the polymer (B).
[0067] Examples of the divalent organic group in the above formula Y5 include the divalent organic groups exemplified in the above Y4. From the viewpoint of reducing residual images derived from residual DC, the polymer (B) is preferably a polymer containing a repeating unit in which Y5 is a divalent organic group selected from the group consisting of the diamine having the above nitrogen atom-containing structure, 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, the divalent organic group derived from the above diamine having a carboxy group, and the divalent organic group represented by the above formula (H) (these are also collectively referred to as specific divalent organic groups).
[0068] From the viewpoint of reducing afterimages caused by residual DC, polymer (B) may contain repeating units in which Y5 is the specific divalent organic group in an amount of 1 mol % or more, or 5 mol % or more, of all repeating units contained in polymer (B).
[0069] From the viewpoint of reducing afterimages caused by residual DC, the content ratio of polymer (A) to polymer (B) in terms of the mass ratio of [polymer (A)] / [polymer (B)] may be 10 / 90 to 90 / 10, 20 / 80 to 90 / 10, or 20 / 80 to 80 / 20.
[0070] <Method for producing polymer (A) and polymer (B)> The polyimide precursors (polyamic acid esters, polyamic acids) which are the polymer (A) and polymer (B) used in the present invention, and the polyimides which are imidized polymers thereof, can be synthesized by known methods, for example, as described in International Publication WO2013 / 157586. Specifically, it is synthesized by reacting a diamine component with a tetracarboxylic acid derivative component in a solvent (condensation polymerization). The tetracarboxylic acid derivative component may be tetracarboxylic acid dianhydride or a derivative thereof (tetracarboxylic acid dihalide, tetracarboxylic acid diester, or tetracarboxylic acid diester dihalide). When a part of the polymer (A) or (B) contains an amic acid structure, for example, a polymer having an amic acid structure (polyamic acid) can be obtained by reacting a tetracarboxylic acid dianhydride component with a diamine component. The solvent is not particularly limited as long as it dissolves the produced polymer.
[0071] The diamine component and the tetracarboxylic acid derivative component for obtaining the polyimide precursor of the polymer (A) are selected and used according to the repeating units represented by the above formulas (1), (2), (2'), (3), and (4) contained in the polymer (A) so as to obtain the structure of such repeating units. For example, when polymer (A) has a repeating unit represented by formula (1), a diamine having a structure of -N(Z)-Y1-N(Z)- (wherein Y1 and Z are defined as above) is used as the diamine component, and a tetracarboxylic acid derivative having a structure of the following formula (g) (wherein R1 to R4 are defined as above) is used as the tetracarboxylic acid derivative component. [ka]
[0072] The polyamic acid ester can be obtained by a known method, for example, [I] a method of reacting the polyamic acid obtained by the above-mentioned method with an esterifying agent, [II] a method of reacting a tetracarboxylic acid diester with a diamine, or [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine. Methods for obtaining polyimide include thermal imidization in which a solution containing a polyimide precursor such as polyamic acid or polyamic acid ester obtained by the above reaction is heated as is, and catalytic imidization in which a catalyst is added to the above solution.
[0073] <Polymer solution viscosity and molecular weight> The polyamic acid, polyamic acid ester, and polyimide used in the present invention preferably have a solution viscosity of, for example, 10 to 1000 mPa·s when made into a solution of 10 to 15% by mass from the viewpoint of workability, but are not particularly limited thereto. The solution viscosity (mPa·s) of the above polymer is a value measured at 25°C using an E-type rotational viscometer for a polymer solution of 10 to 15% by mass prepared using a good solvent for the polymer (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.). The polystyrene-equivalent weight average molecular weight (Mw) of the polyamic acid, polyamic acid ester, and polyimide measured by gel permeation chromatography (GPC) is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000. The molecular weight distribution (Mw / Mn), which is expressed as the ratio of Mw to the polystyrene-equivalent number average molecular weight (Mn) measured by GPC, is preferably 15 or less, and more preferably 10 or less. With the molecular weight in this range, good alignment and stability of the liquid crystal display element can be ensured.
[0074] <Liquid crystal alignment agent> The liquid crystal alignment agent of the present invention contains a polymer (A) and, if necessary, a polymer (B). The liquid crystal alignment agent of the present invention may contain other polymers in addition to the polymer (A) and the polymer (B). Examples of the other polymers include polyesters, polyamides, polyureas, polyorganosiloxanes, cellulose derivatives, polyacetals, polystyrene or its derivatives, poly(styrene-phenylmaleimide) derivatives, and poly(meth)acrylates.
[0075] The liquid crystal aligning agent is used to prepare a liquid crystal alignment film, and takes the form of a coating liquid from the viewpoint of forming a uniform thin film. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent. In this case, the concentration of the polymer in the liquid crystal aligning agent can be appropriately changed depending on the thickness of the coating film to be formed. From the viewpoint of forming a uniform and defect-free coating film, it is preferably 1% by mass or more, and from the viewpoint of storage stability of the solution, it is preferably 10% by mass or less. A particularly preferable concentration of the polymer is 2 to 8% by mass.
[0076] The organic solvent contained in the liquid crystal alignment agent is not particularly limited as long as the polymer component is dissolved uniformly. Specific examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethylsulfoxide, γ-butyrolactone, 1,3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide (collectively referred to as "good solvents"). Among them, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, or γ-butyrolactone is preferred. The content of the good solvent is preferably 20 to 99 mass %, more preferably 20 to 90 mass %, and particularly preferably 30 to 80 mass %, of the total solvent contained in the liquid crystal aligning agent.
[0077] In addition, the organic solvent contained in the liquid crystal alignment agent is preferably a mixed solvent containing the above-mentioned solvent and a solvent (also called a poor solvent) that improves the coating property when applying the liquid crystal alignment agent and the surface smoothness of the coating film. Specific examples of the poor solvent to be used in combination are shown below, but are not limited thereto. For example, diisopropyl ether, diisobutyl ether, diisobutyl carbinol (2,6-dimethyl-4-heptanol), ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, ethylene glycol monobutyl ether, ethylene glycol monoisoamyl ether, ethylene glycol monohexyl ether, propylene glycol monobutyl ether, 1-(2-butoxyethoxy)-2-propanol, 2-(2-butoxy)-2-propanol, Examples of the ethoxy)-1-propanol, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol monoacetate, ethylene glycol diacetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, propylene glycol diacetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, n-butyl lactate, isoamyl lactate, diethylene glycol monoethyl ether, diisobutyl ketone (2,6-dimethyl-4-heptanone), and the like.
[0078] Of these, diisobutyl carbinol, propylene glycol monobutyl ether, propylene glycol diacetate, diethylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, or diisobutyl ketone is preferred.
[0079] The content of the poor solvent is preferably 1 to 80 mass % of the total solvent contained in the liquid crystal alignment agent, more preferably 10 to 80 mass %, particularly preferably 20 to 70 mass %. The type and content of the poor solvent are appropriately selected depending on the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent. Preferred combinations of good and poor solvents include N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, and propylene glycol monobutyl ether, N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone, and diethylene glycol diethyl ether, and N-methyl-2-pyrrolidone and γ- butyrolactone, propylene glycol monobutyl ether, and diisobutyl ketone, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisopropyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisobutyl carbinol, N-methyl-2-pyrrolidone, γ-butyrolactone, and dipropylene glycol dimethyl ether, and N-methyl-2-pyrrolidone, propylene glycol monobutyl ether, and dipropylene glycol dimethyl ether.
[0080] The liquid crystal alignment agent of the present invention may additionally contain components other than the polymer component and the organic solvent (hereinafter also referred to as additive components). Examples of such additive components include adhesion assistants for increasing the adhesion between the liquid crystal alignment film and the substrate or between the liquid crystal alignment film and the sealant, compounds for increasing the strength of the liquid crystal alignment film (hereinafter also referred to as crosslinking compounds), compounds for promoting imidization, and dielectrics and conductive substances for adjusting the dielectric constant and electrical resistance of the liquid crystal alignment film.
[0081] From the viewpoint of exhibiting good resistance to AC afterimages and highly improving film strength, the crosslinkable compound may be at least one compound selected from the group consisting of compounds having at least one group selected from the group consisting of an oxiranyl group, an oxetanyl group, a protected isocyanate group, a protected isothiocyanate group, a group containing an oxazoline ring structure, a group containing a Meldrum's acid structure, a cyclocarbonate group, and a group represented by the following formula (d), and a compound represented by the following formula (e) (hereinafter these may be collectively referred to as compound (C)). [ka] (In formula (d), R2 and R3 each independently represent a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or "*-CH2-OH". * represents a bond. In formula (e), A represents an (m+n)-valent organic group having an aromatic ring, R represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, m is 1 to 6, and n is 0 to 4. The aromatic ring of A may be substituted with a monovalent group, and specific examples of the monovalent group include Ar in the above formula (O2). 2’ Examples of the monovalent groups include those shown as the substituents of
[0082] Specific examples of the compound having an oxiranyl group include compounds having two or more oxiranyl groups, such as the compounds described in paragraph
[0037] of JP-A-10-338880 and compounds having a triazine ring skeleton described in International Publication WO2017 / 170483. Among these, the compound may be a compound containing a nitrogen atom, such as N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, or a compound represented by any one of the following formulas (r-1) to (r-3). [ka]
[0083] Specific examples of the compound having an oxetanyl group include compounds having two or more oxetanyl groups described in paragraphs
[0170] to
[0175] of WO 2011 / 132751. Specific examples of the compound having a protected isocyanate group include the compound having two or more protected isocyanate groups described in paragraphs
[0046] to
[0047] of JP 2014-224978 A, and the compound having three or more protected isocyanate groups described in paragraphs
[0119] to
[0120] of WO 2015 / 141598 A. The compound may be a compound represented by any of the following formulas (bi-1) to (bi-3). [ka]
[0084] Specific examples of compounds having a protected isothiocyanate group include compounds having two or more protected isothiocyanate groups described in JP 2016-200798 A. Specific examples of the compound having a group containing an oxazoline ring structure include compounds containing two or more oxazoline ring structures described in paragraph
[0115] of JP 2007-286597 A.
[0085] Specific examples of the compound having a group containing a Meldrum's acid structure include compounds having two or more Meldrum's acid structures described in International Publication WO2012 / 091088. Specific examples of the compound having a cyclocarbonate group include the compounds described in International Publication WO2011 / 155577. Examples of the alkyl group having 1 to 3 carbon atoms for R2 and R3 in the group represented by the above formula (d) include a methyl group, an ethyl group, a propyl group, and an isopropyl group.
[0086] Specific examples of the compound having a group represented by the above formula (d) include compounds having two or more groups represented by the above formula (d) described in International Publication No. WO2015 / 072554 and paragraph
[0058] of JP 2016-118753 A, and compounds described in JP 2016-200798 A. The compound may be a compound represented by any of the following formulae (hd-1) to (hd-8). [ka]
[0087] Examples of the (m+n)-valent organic group having an aromatic ring in A of the above formula (e) include an (m+n)-valent aromatic hydrocarbon group having 6 to 30 carbon atoms, an (m+n)-valent organic group to which an aromatic hydrocarbon group having 6 to 30 carbon atoms is bonded directly or via a linking group, and an (m+n)-valent group having an aromatic heterocycle. Examples of the aromatic hydrocarbon group include benzene and naphthalene. Examples of the aromatic heterocycle include the structures exemplified for the nitrogen atom-containing heterocycle. Examples of the linking group include -NR- (R represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms), an alkylene group having 1 to 10 carbon atoms, or a group obtained by removing one hydrogen atom from the alkylene group, and a divalent or trivalent cyclohexane ring. Any hydrogen atom in the alkylene group may be substituted with an organic group such as a fluorine atom or a trifluoromethyl group. Examples of the alkyl group having 1 to 5 carbon atoms for R in the above formula (e) include the alkyl groups exemplified for R1 to R4 in the above formula (1). Specific examples of the above formula (e) include the compounds described in International Publication WO2010 / 074269 and compounds represented by any of the following formulae (e-1) to (e-10). [ka]
[0088] The above compounds are examples of crosslinkable compounds, and are not limited thereto. For example, components other than those described above are disclosed on pages 53
[0105] to 55
[0116] of International Publication No. 2015 / 060357. In addition, two or more types of crosslinkable compounds may be combined. The content of the crosslinkable compound in the liquid crystal aligning agent of the present invention is preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the polymer component contained in the liquid crystal aligning agent, and from the viewpoint of proceeding with the crosslinking reaction and exhibiting good resistance to AC afterimages, it is more preferably 1 to 15 parts by mass.
[0089] Examples of the adhesion aid include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxy ... triethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyltrimethoxysilane, N-benzyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-bis(oxyethylene)-3-aminopropyltrimethoxysilane, N-bis(oxyethylene)-3-aminopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,Examples of silane coupling agents include 4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane. When a silane coupling agent is used, the amount is preferably 0.1 to 30 parts by mass, and more preferably 0.1 to 20 parts by mass, per 100 parts by mass of the polymer component contained in the liquid crystal alignment agent, from the viewpoint of exhibiting good resistance to AC afterimages.
[0090] The compound for promoting the imidization is preferably a compound having a basic site (e.g., a primary amino group, an aliphatic heterocycle (e.g., a pyrrolidine skeleton), an aromatic heterocycle (e.g., an imidazole ring, an indole ring), or a guanidino group, etc.) (excluding the crosslinkable compound and the adhesion aid), or a compound that generates the basic site when baked. More preferably, it is a compound that generates the basic site when baked, and a preferred specific example is an amino acid in which a part or all of the basic site of the amino acid is protected. Specific examples of the amino acid include glycine, alanine, cysteine, methionine, asparagine, glutamine, valine, leucine, phenylalanine, tyrosine, tryptophan, proline, hydroxyproline, arginine, histidine, lysine, and ornithine. A more preferred specific example of the compound for promoting the imidization is N-α-(9-fluorenylmethoxycarbonyl)-N-τ-(tert-butoxycarbonyl)-L-histidine.
[0091] <Method of manufacturing liquid crystal alignment film> The method for producing a liquid crystal alignment film using the liquid crystal alignment agent of the present invention is characterized by sequentially carrying out the steps of applying the above-mentioned liquid crystal alignment agent (step (1)), heating the applied liquid crystal alignment agent to obtain a film (step (2)), irradiating the film obtained in step (2) with polarized ultraviolet light (step (3)), and baking the film obtained in step (3) at a temperature of 100°C or higher and at a temperature higher than that of step (2) (step (4)).
[0092] <Process (1)> The substrate to which the liquid crystal alignment agent used in the present invention is applied is not particularly limited as long as it is a highly transparent substrate, and a glass substrate, a silicon nitride substrate, a plastic substrate such as an acrylic substrate or a polycarbonate substrate, etc. can also be used. In this case, it is preferable to use a substrate on which an ITO electrode for driving the liquid crystal is formed from the viewpoint of simplifying the process. In addition, in a reflective liquid crystal display element, an opaque material such as a silicon wafer can be used for only one substrate, and in this case, a light-reflecting material such as aluminum can be used for the electrode. The method of applying the liquid crystal alignment agent is not particularly limited, but in industry, it is generally performed by screen printing, offset printing, flexographic printing, inkjet printing, etc. Other application methods include a dip method, a roll coater method, a slit coater method, a spinner method, a spray method, etc., and these may be used depending on the purpose.
[0093] <Process (2)> Step (2) is a step of heating the liquid crystal alignment agent applied on the substrate to form a film. Specifically, the liquid crystal alignment agent applied on the substrate in step (1) can be heated by a heating means such as a hot plate, a heat circulation type oven, or an IR (infrared) type oven to evaporate the solvent or to thermally imidize the amic acid or amic acid ester in the polymer. The heating step of the liquid crystal alignment agent applied on the substrate in step (1) can be performed at any temperature and time, and may be performed multiple times. The heating temperature can be, for example, 40 to 180°C, and from the viewpoint of shortening the process, it is preferably performed at 40 to 150°C, and more preferably at 40 to 120°C. The heating time is not particularly limited, but can be 1 to 10 minutes or 1 to 5 minutes. When thermally imidizing the amic acid or amic acid ester in the polymer, a heating step can be performed at a temperature range of, for example, 190 to 250°C or 200 to 240°C after the above heating step. The heating time is not particularly limited, but may be 5 to 40 minutes, or 5 to 30 minutes.
[0094] <Process (3)> Step (3) is a step of irradiating the film obtained in step (2) with polarized ultraviolet light. The wavelength of the ultraviolet light is preferably 200 to 400 nm, and more preferably, ultraviolet light having a wavelength of 200 to 300 nm is used. In order to improve the liquid crystal alignment, the substrate on which the liquid crystal alignment film is coated may be irradiated with ultraviolet light while being heated at 50 to 250°C. The irradiation dose of the ultraviolet light is 1 to 10,000 mJ / cm. 2 is preferable, and 100 to 5,000 mJ / cm 2 The liquid crystal alignment film thus prepared can stably align liquid crystal molecules in a certain direction. The higher the extinction ratio of the polarized UV light, the higher the anisotropy that can be imparted, which is preferable. Specifically, the extinction ratio of the linearly polarized UV light is preferably 10:1 or more, and more preferably 20:1 or more.
[0095] <Process (4)> Step (4) is a step of baking the film obtained in step (3) at 100° C. or higher and at a temperature higher than that in step (2). The baking temperature is not particularly limited as long as it is 100° C. or higher and higher than the baking temperature in step (2), but is preferably 150 to 300° C., more preferably 150 to 250° C., and even more preferably 200 to 250° C. The baking time is preferably 5 to 120 minutes, more preferably 5 to 60 minutes, and even more preferably 5 to 30 minutes. The thickness of the liquid crystal alignment film after baking is preferably 5 to 300 nm, more preferably 10 to 200 nm, since if it is too thin, the reliability of the liquid crystal display element may decrease.
[0096] Furthermore, after carrying out either the above step (3) or (4), the obtained liquid crystal alignment film can be subjected to a contact treatment using water or a solvent. The solvent used in the contact treatment is not particularly limited as long as it dissolves the decomposition product generated from the liquid crystal alignment film by irradiation with ultraviolet light. Specific examples include water, methanol, ethanol, 2-propanol, acetone, methyl ethyl ketone, 1-methoxy-2-propanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, methyl lactate, diacetone alcohol, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, propyl acetate, butyl acetate, and cyclohexyl acetate. Among them, water, 2-propanol, 1-methoxy-2-propanol, and ethyl lactate are preferred from the viewpoint of versatility and solvent safety, and water, 1-methoxy-2-propanol, and ethyl lactate are more preferred. The solvent may be one type or a combination of two or more types.
[0097] The contact treatment, i.e., the treatment of the liquid crystal alignment film irradiated with polarized ultraviolet light with water or a solvent, may be immersion treatment or spray treatment (also called spray treatment). The treatment time in these treatments is preferably 10 seconds to 1 hour from the viewpoint of efficiently dissolving the decomposition products generated from the liquid crystal alignment film by ultraviolet light. In particular, immersion treatment for 1 to 30 minutes is preferable. The solvent during the contact treatment may be at room temperature or heated, preferably 10 to 80°C, more preferably 20 to 50°C. In addition, ultrasonic treatment or the like may be performed as necessary from the viewpoint of the solubility of the decomposition products. After the contact treatment, it is preferable to rinse the liquid crystal alignment film with a low boiling point solvent such as water, methanol, ethanol, 2-propanol, acetone, or methyl ethyl ketone, or to bake the liquid crystal alignment film. Either rinsing or baking may be performed, or both may be performed. The baking temperature is preferably 150 to 300°C, more preferably 180 to 250°C, and even more preferably 200 to 230°C. The baking time is preferably 10 seconds to 30 minutes, and more preferably 1 to 10 minutes.
[0098] <Liquid crystal alignment film> The liquid crystal alignment film of the present invention is obtained from the above liquid crystal aligning agent. The liquid crystal alignment film of the present invention is suitable as a liquid crystal alignment film for a liquid crystal display element of a horizontal electric field mode such as an IPS mode or an FFS mode, and is particularly useful as a liquid crystal alignment film for a liquid crystal display element of an FFS mode.
[0099] <Liquid crystal display element> The liquid crystal display element of the present invention comprises the above-mentioned liquid crystal alignment film. A liquid crystal display element can be obtained by preparing a substrate having a liquid crystal alignment film obtained from the liquid crystal aligning agent of the present invention, and then preparing a liquid crystal cell by a known method, and using the liquid crystal cell. As an example of a method for fabricating a liquid crystal cell, a liquid crystal display element having a passive matrix structure will be described below. However, a liquid crystal display element having an active matrix structure in which a switching element such as a TFT (Thin Film Transistor) is provided in each pixel portion constituting an image display may also be used.
[0100] Specifically, transparent glass substrates are prepared, and a common electrode is provided on one substrate, and a segment electrode is provided on the other substrate. These electrodes may be, for example, ITO electrodes, and are patterned to display a desired image. Next, an insulating film is provided on each substrate so as to cover the common electrode and the segment electrode. The insulating film may be, for example, a SiO2-TiO2 film formed by the sol-gel method. Next, a liquid crystal alignment film is formed on each substrate, and one substrate is superimposed on the other substrate so that the liquid crystal alignment film faces each other, and the periphery is bonded with a sealant. In order to control the gap between the substrates, a spacer is usually mixed into the sealant, and it is also preferable to scatter spacers for controlling the gap between the substrates on the inner surface where the sealant is not provided. An opening is provided in a part of the sealant so that liquid crystal can be filled from the outside. Next, a liquid crystal material is injected into the space surrounded by the two substrates and the sealant through the opening provided in the sealant, and then the opening is sealed with an adhesive. For the injection, a vacuum injection method or a method utilizing capillary action in the atmosphere may be used. The liquid crystal material may be either a positive type liquid crystal material or a negative type liquid crystal material. Next, a polarizing plate is installed. Specifically, a pair of polarizing plates is attached to the surface of the two substrates opposite to the liquid crystal layer.
[0101] By using the manufacturing method of the present invention, it is possible to suppress image retention caused by long-term AC driving in liquid crystal display elements of IPS driving type or FFS driving type. In addition, by carrying out heating in a temperature range of 40 to 150°C in step (2) and then carrying out step (3), a liquid crystal alignment film can be obtained with fewer steps than in the past. The liquid crystal alignment agent of the present invention can be particularly preferably used in a manufacturing method of a liquid crystal alignment film including a step of removing an organic solvent in a temperature range of 40 to 150°C in step (2) and then carrying out step (3). EXAMPLES
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. The abbreviations of compounds and the measuring methods of each property are as follows. (solvent) NMP: N-methyl-2-pyrrolidone BCS: butyl cellosolve; (Diamine) DA-1 to DA-12: Compounds represented by the following formulas (DA-1) to (DA-12), (Tetracarboxylic acid dianhydride) CA-1 to CA-2: Compounds represented by the following formulae (CA-1) to (CA-2), (Additives) C-1: A compound represented by the following formula (C-1): S-1: a compound represented by the following formula (S-1): F-1: A compound represented by the following formula (F-1):
[0103] [ka]
[0104] [ka]
[0105] [ka]
[0106] <Measurement of imidization rate> 20 mg of polyimide powder was placed in an NMR sample tube (NMR sampling tube standard, φ5 (Kusano Scientific Co., Ltd.)), deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS (tetramethylsilane) mixture) (0.53 mL) was added, and the mixture was completely dissolved by ultrasonication. This solution was measured by 500 MHz proton NMR using an NMR measurement device (JNW-ECA500) (JEOL Datum Co., Ltd.). The imidization rate was calculated by the following formula using the proton peak integrated value of this proton and the proton peak integrated value of the proton peak derived from the NH group of the amic acid that appears around 9.5 ppm to 10.0 ppm. Imidization rate (%) = (1-α·x / y) × 100 In the above formula, x is the integrated value of the proton peak derived from the NH group of the amic acid, y is the integrated value of the peak of the reference proton, and α is the ratio of the number of reference protons to one NH group proton of the amic acid in the case of polyamic acid (imidization rate 0%).
[0107] [Polymer synthesis example] <Synthesis Example 1> 9.34g (38.3mmol) of DA-1 and 1.60g (6.75mmol) of DA-3 were weighed out into a 200mL four-neck flask equipped with a stirrer and a nitrogen inlet tube, and NMP was added to the mixture so that the concentration was 12% by mass. The mixture was stirred and dissolved while feeding nitrogen. 9.28g (41.4mmol) of CA-1 was added while stirring this diamine solution, and NMP was added to the mixture so that the concentration was 12% by mass. The mixture was stirred at 40°C for 24 hours to obtain a polyamic acid solution. 35g (9.3mmol) of the obtained polyamic acid solution was taken in a 100mL four-neck flask equipped with a stirrer and a nitrogen inlet tube, 11.7g of NMP was added, and the mixture was stirred for 30 minutes. 2.86g of acetic anhydride (3 equivalents relative to the molar amount of polyamic acid) and 0.74g of pyridine (equivalent to the molar amount of polyamic acid) were added to the obtained solution, and the mixture was heated at 55°C for 3 hours to perform chemical imidization. The obtained reaction solution was poured into 150mL of methanol while stirring, the precipitate was filtered off, and the resin powder was washed by performing the same operation twice, and then dried under reduced pressure at 60°C for 12 hours to obtain a polyimide resin powder. The imidization rate of this polyimide resin powder was 71%. 3.60g of the obtained polyimide resin powder was taken in a 100mL Erlenmeyer flask, NMP was added so that the solid concentration was 12%, and the mixture was stirred and dissolved at 70°C for 24 hours to obtain a polyimide solution (PI-1).
[0108] <Synthesis Examples 2 to 11> Polyimide solutions (PI-2) to (PI-12) were obtained in the same manner as in Synthesis Example 1, except that the types and amounts of monomers used were changed as shown in Table 1 below. In Table 1, the numbers in parentheses indicate the blending ratio (parts by mole) of each compound relative to 100 parts by mole of the total amount of tetracarboxylic acid derivatives used in the synthesis for the tetracarboxylic acid components, and the blending ratio (parts by mole) of each compound relative to 100 parts by mole of the total amount of diamines used in the synthesis for the diamine components. The organic solvents indicate the blending ratio (parts by mass) of each organic solvent relative to 100 parts by mass of the total amount of organic solvents used in the preparation of the polyimide solution.
[0109] <Synthesis Example 13> 2.69g (9.0mmol) of DA-6 and 7.17g (36.0mmol) of DA-11 were weighed out into a 200mL four-neck flask equipped with a stirrer and a nitrogen inlet tube, and NMP was added to the mixture so that the concentration was 12% by mass. The mixture was stirred and dissolved while feeding nitrogen. 12.2g (41.4mmol) of CA-2 was added while stirring this diamine solution, and NMP was added to the mixture so that the concentration was 12% by mass. The mixture was stirred at 70°C for 24 hours to obtain a polyamic acid solution (PAA-1).
[0110] [Table 1]
[0111] [Preparation of liquid crystal alignment agent] <Comparative Example 1> In a sample tube containing a stirrer, the polyimide solution (PI-1) obtained in Synthesis Example 1 and the polyamic acid solution (PAA-1) obtained in Synthesis Example 13 were mixed so that the polymer solid content ratio was 50:50 by mass, NMP and BCS were added to dilute, and S-1, C-1 and F-1 were added in amounts of 1 part by mass, 10 parts by mass and 15 parts by mass, respectively, per 100 parts by mass of the total polymer solid content, and the mixture was stirred for 30 minutes. After stirring, a liquid crystal alignment agent (R1) was obtained in which the polymer solid content ratio of polyimide (PI-1) and polyamic acid (PAA-1) was 50:50, the polymer solid content concentration was 6% by mass, and the solvent composition was NMP:BCS=80:20 by mass.
[0112] <Comparative Examples 2 to 5, Examples 1 to 14> Except for changing the polymer components used as shown in Table 2 below, the same procedure as in Comparative Example 1 was carried out to obtain liquid crystal alignment agents (R2) to (R5) and liquid crystal alignment agents (1) to (14). In Table 2, the numbers in parentheses indicate the blending ratio (parts by mass) of each polymer component or additive relative to 100 parts by mass of the total polymer components used in the preparation of the liquid crystal alignment agent for the polymer and additive, respectively. For the organic solvent, the blending ratio (parts by mass) of each organic solvent relative to 100 parts by mass of the total amount of the organic solvent contained in the liquid crystal alignment agent is indicated.
[0113] [Table 2]
[0114] Using the liquid crystal alignment agent obtained as described above, an FFS drive liquid crystal cell was produced according to the procedure described below, and its characteristics were evaluated.
[0115] [FFS drive liquid crystal cell configuration] The liquid crystal cell for Fringe Field Switching (FFS) mode is a set of a first glass substrate on which an FOP (Finger on Plate) electrode layer consisting of a planar common electrode, an insulating layer, and a comb-shaped pixel electrode is formed on the surface, and a second glass substrate on which a columnar spacer with a height of 3.5 μm is formed on the surface and an ITO film for antistatic is formed on the back surface. The pixel electrode has a comb shape in which multiple electrode elements with a width of 3 μm and bent at an internal angle of 160° at the center are arranged in parallel with a 6 μm gap, and one pixel has a first region and a second region with a line connecting the bent parts of the multiple electrode elements as the boundary. The liquid crystal alignment film formed on the first glass substrate is oriented so that the direction dividing the interior angles of the pixel bends is perpendicular to the alignment direction of the liquid crystal, and the liquid crystal alignment film formed on the second glass substrate is oriented so that the alignment direction of the liquid crystal on the first substrate coincides with the alignment direction of the liquid crystal on the second substrate when the liquid crystal cell is fabricated.
[0116] [Preparation of liquid crystal cells] A liquid crystal alignment agent filtered through a 1.0 μm filter was applied to the surface of each of the above-mentioned pair of glass substrates by spin coating, and then dried on a hot plate at 80° C. for 2 minutes. After that, linearly polarized ultraviolet light with an extinction ratio of 26:1 and a wavelength of 254 nm was irradiated on the coating surface through a polarizer at 150 to 350 mJ / cm. 2 The substrate was then irradiated and then baked in a hot air circulating oven at 230° C. for 30 minutes to obtain two substrates with a liquid crystal alignment film having a thickness of 100 nm. Next, a sealant was printed on one of the pair of substrates with liquid crystal alignment film, and the other substrate was attached so that the liquid crystal alignment film faces each other, and the sealant was cured to prepare an empty cell. Liquid crystal (MLC-3019, manufactured by Merck) was vacuum-injected into this empty cell at room temperature by a reduced pressure injection method, and the injection port was sealed to obtain an FFS-driven liquid crystal cell. The obtained liquid crystal cell was then heated at 120°C for 1 hour and left overnight before being used for each evaluation.
[0117] <Liquid crystal alignment evaluation> The evaluation was performed by using liquid crystal cells before the ISO treatment, defining those with initial flow alignment as "bad" and those without initial flow alignment as "good". <Evaluation of in-plane uniformity of contrast> The twist angle of the liquid crystal display element was evaluated using OPTIPRO-micro manufactured by Shintech Co., Ltd. The fabricated liquid crystal cell was placed on the measurement stage, and 20 points within the first pixel plane were measured without applying voltage, and the standard deviation was calculated. The evaluation was performed by defining a twist angle standard deviation of 0.5 or more as "poor" and one less than 0.5 as "good."
[0118] <Evaluation Results> Table 3 shows the evaluation results of the liquid crystal display elements obtained by using the liquid crystal alignment agents (1) to (14) and (R1) to (R5) obtained in the above Examples 1 to 14 and Comparative Examples 1 to 5.
[0119] [Table 3] [Industrial Applicability]
[0120] The liquid crystal aligning agent of the present invention is widely used in liquid crystal display elements of vertical electric field modes such as TN mode and VA mode, and particularly in horizontal electric field modes such as IPS mode and FFS mode.
[0121] In addition, the entire contents of the specifications, claims and abstracts of Japanese Patent Application No. 2020-039386 filed on March 6, 2020 and Japanese Patent Application No. 2020-123011 filed on July 17, 2020 are hereby incorporated by reference as the disclosure of the specification of the present invention.
Claims
1. A liquid crystal alignment film comprising at least one polymer selected from the group consisting of a polyimide precursor having a repeating unit (a4) represented by the following formula (4) and an imidized polymer thereof: [Formula 1] (In formula (4), X 4 represents a tetravalent organic group, and R and Z each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 4 represents a divalent organic group represented by the following formula (H), a divalent organic group represented by the following formula (O), a divalent organic group represented by the following formula (O2), a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate protecting group)" in the molecule, or a divalent organic group represented by any of the following formulas (g-1) to (g-5). [chemical 2] (In formula (H), Q 1 represents a divalent organic group having 1 to 18 carbon atoms and having *1-NH-C(=O)-*1 or *1-NH-C(=O)-NH-*1. *1 represents a bond bonded to a carbon atom.) [C3] In formula (O), each Ar independently represents a benzene ring, a biphenyl structure, or a naphthalene ring, and at least one of the two Ar represents a naphthalene ring. Any hydrogen atom on the ring may be replaced with a halogen atom or a monovalent organic group. Q 2 Ha-(CH 2 ) n -(n is an integer of 2 to 18), or the -(CH 2 ) n represents a group in which a portion of - is replaced with -O-, -C(=O)-, or -O-C(=O)-. [C4] (In formula (O2), Ar 2’ represents a benzene ring, and any hydrogen atom on the ring may be replaced with a halogen atom or a monovalent organic group. 2’ is a single bond, -O-, -C(=O)-, -O-C(=O)-, -(CH 2 ) n -(n is 2 to 18), or the -(CH 2 ) n represents a group in which a part of - is replaced by -O-, -C(=O)- or -O-C(=O)-. m is an integer of 0 to 2. 2’ , Q 2’ When multiple are present, they may be the same or different.) [C5]
2. The Y 4 a repeating unit represented by formula (4) which is a divalent organic group represented by formula (H); The Y 4 The liquid crystal alignment film according to claim 1, comprising at least one polymer selected from the group consisting of a polyimide precursor having a repeating unit represented by formula (4), which is a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate-based protecting group)" in the molecule, and an imidized polymer thereof.
3. The Y 4 a repeating unit represented by formula (4) which is a divalent organic group represented by formula (H); The Y 4 A repeating unit represented by formula (4) which is a divalent organic group having 6 to 30 carbon atoms and having a group "-N(D)- (D represents a carbamate protecting group)" in the molecule, The Y 4 and a repeating unit represented by formula (4) which is a divalent organic group represented by formula (O), and at least one polymer selected from the group consisting of a polyimide precursor having the repeating unit represented by formula (4) and an imidized polymer thereof.
4. 4. The liquid crystal alignment film according to claim 1, wherein the imidization rate of the polyimide contained in the polymer is 71% or more.
5. The liquid crystal alignment film according to any one of claims 1 to 4, comprising a polymer (B) other than the polymer, which does not have both a repeating unit represented by formula (4) which is a divalent organic group represented by formula (H) and a repeating unit represented by formula (4) which is a divalent organic group represented by formula (O) in the same molecule.
6. The liquid crystal alignment film according to claim 5, wherein the polymer (B) is a polymer having at least one repeating unit selected from the group consisting of a repeating unit (b1) represented by the following formula (5) and an imidized structural unit of the repeating unit (b1): [C6] (In the formula, X 5 is a tetravalent organic group, Y 5 is a divalent organic group. Each Z independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group. R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
7. The Y 5 is a divalent organic group selected from the group consisting of a diamine having a nitrogen atom-containing structure, 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, a divalent organic group derived from a diamine having a carboxy group, and a divalent organic group represented by formula (H). The liquid crystal alignment film according to claim 6.
8. 8. The liquid crystal alignment film according to claim 7, wherein the diamine having a nitrogen atom-containing structure is a diamine having at least one nitrogen atom-containing structure selected from the group consisting of a nitrogen atom-containing heterocycle, a secondary amino group, and a tertiary amino group.
9. The liquid crystal alignment film according to claim 8 , wherein the secondary amino group and the tertiary amino group are represented by the following formula (n): [C7] (In formula (n), R represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. "*1" represents a bond bonded to the hydrocarbon group.)
10. The liquid crystal alignment film according to any one of claims 1 to 9, further comprising a crosslinkable compound.
11. The divalent organic group represented by the formula (H) is a divalent organic group represented by any one of the following formulas (h-1) to (h-6): Liquid crystal alignment film according to any one of claims 1 to 10. [C8]
12. The divalent organic group represented by the formula (O) is a divalent organic group represented by any one of the following formulas (o-1) to (o-6): Liquid crystal alignment film according to any one of claims 1 to 10. [C9]
13. The divalent organic group represented by the formula (O2) is a divalent organic group represented by any one of the following formulas (o2-1) to (o2-11): [C10]
14. The divalent organic group having 6 to 30 carbon atoms and having the group "-N(D)- (D represents a carbamate-based protecting group)" in the molecule is a divalent organic group having a partial structure represented by the following formula (3-1), or a divalent organic group represented by the following formula (3-2). The liquid crystal alignment film according to any one of claims 1 to 13. [C11] (In the formula, Q 5 is a single bond, -(CH 2 ) n -(n is 1 to 20), or the -(CH 2 ) n Any of -CH 2 - is -O-, -COO-, -OCO-, -NQ 9 --, --NQ 9 CO-, -CONQ 9 --, --NQ 9 -CO-NQ 10 --, --NQ 9 is a group replaced by —COO— or —O—COO—, 9 and Q. 10 each independently represents a hydrogen atom or a monovalent organic group. Q 6 and Q. 7 Each independently represents -H, -NHD, -N(D) 2 , a group having -NHD, -N(D) 2 Q represents a group having the formula: 8 -NHD, -N(D) 2 , a group having -NHD, -N(D) 2 D represents a carbamate protecting group. 5 , Q 6 and Q. 7 At least one of the groups has a carbamate-based protecting group in the group.
15. The divalent organic group having 6 to 30 carbon atoms and having the group "-N(D)- (D represents a carbamate-based protecting group)" in the molecule is a structure represented by any one of the following formulas (Y3-1) to (Y3-5). The liquid crystal alignment film according to any one of claims 1 to 14. [C12] (In each formula, Boc represents a tert-butoxycarbonyl group, and * represents a bond.)
16. The X 4 The liquid crystal alignment film according to any one of claims 1 to 15, wherein is a tetravalent organic group represented by the following formula (g): [C13] (R 1 , R 2 , R 3 , R 4 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms containing a fluorine atom, or a phenyl group; R 1 ~R 4 At least one of represents a group other than a hydrogen atom as defined above.)
17. In the formula (g), R 1 and R 4 is a methyl group, R 2 and R 3 The liquid crystal alignment film according to claim 16 , wherein is a hydrogen atom.
18. A liquid crystal display device comprising the liquid crystal alignment film according to any one of claims 1 to 17.
19. A method for producing a liquid crystal alignment film according to any one of claims 1 to 17, comprising the following steps (1) and (2): Step (1): A step of heating a liquid crystal alignment agent in a temperature range of 40 to 180° C. to obtain a liquid crystal alignment film. Step (2): A step of irradiating the liquid crystal alignment film obtained in step (1) with polarized ultraviolet light.
20. The method for producing a liquid crystal alignment film according to claim 19, further comprising the following step (3): Step (3): Firing at a temperature of 200 to 250° C. for 5 to 120 minutes.
21. The method for producing a liquid crystal alignment film according to claim 19 or 20, wherein the ultraviolet light has a wavelength of 200 to 300 nm.
22. A liquid crystal display device comprising a liquid crystal alignment film obtained by the method for producing a liquid crystal alignment film according to any one of claims 19 to 21.
Citation Information
Patent Citations
Liquid crystal aligning agent and liquid crystal display using the same
JP2005157346A
Liquid crystal aligning agent, liquid crystal alignment film, liquid crystal element, polymer and diamine
JP2017138575A
Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element using same
WO2018110354A1
Method for orienting liquid crystal
JP1997297313A
Liquid crystal aligning agent for in-plate switching, liquid crystal alignment film and liquid crystal display element using same
WO2015050135A1