Light-emitting element, light-emitting device, electronic device and lighting device
A novel heterocyclic compound forms an exciplex with an aromatic amine to improve luminous efficiency and heat resistance in light-emitting devices, addressing limitations in existing phosphorescent compound-based technologies.
Patent Information
- Application Number
- JP2024150505
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2012-08-03
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing light-emitting devices using phosphorescent compounds face limitations in luminous efficiency, reliability, and cost, with a need for improved materials to enhance performance.
A novel heterocyclic compound is synthesized, combining a pyrimidine ring with a hole-transporting skeleton and an aromatic amine to form an exciplex, which efficiently converts triplet excitation energy into luminescence, improving luminous efficiency and heat resistance.
The novel heterocyclic compound enhances the luminous efficiency and heat resistance of light-emitting elements, leading to long-life and low-power consumption devices.
Smart Images

Figure 2024163181000034 
Figure 2024163181000035 
Figure 2024163181000036
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-emitting element, a light-emitting device, an electronic device, a lighting device, and a heterocyclic compound. [Background technology]
[0002] In recent years, electroluminescence (EL) The basic structure of these light-emitting devices is as follows: The device has a layer containing a light-emitting substance sandwiched between a pair of electrodes. Thus, light emission from the luminescent substance can be obtained.
[0003] Since these light-emitting elements are self-emitting, the pixels have higher visibility than LCD displays. It has the advantage of being simple and does not require a backlight, making it ideal for use as a flat panel display element. In addition, such a light-emitting element can be manufactured to be thin and lightweight. Another major advantage is that it has an extremely fast response time.
[0004] In addition, since these light emitting elements can be formed in a film shape, surface light emission can be obtained. Therefore, a large-area element utilizing surface light emission can be easily formed. This is something that cannot be achieved with point light sources such as incandescent bulbs and LEDs, or linear light sources such as fluorescent lamps. Because of this rare feature, it is also highly useful as a surface light source for lighting applications, etc.
[0005] The light-emitting element that utilizes electroluminescence is either an organic compound or They can be broadly classified according to whether they are organic or inorganic compounds. In the case of an organic EL element having a layer containing the organic compound, applying a voltage to the light emitting element By this, electrons flow from the cathode and holes flow from the anode. The injected electrons and holes excite the light-emitting organic compound, causing a current to flow. The excited organic compound emits light.
[0006] The types of excited states that organic compounds can form are singlet excited states and triplet excited states. It is possible to obtain a singlet excited state (S * ) is emitted from the triplet excited state (T * ) from The light that is generated is called phosphorescence. The statistical generation rate of phosphorescence in a light-emitting device is S * :T * It is believed that the ratio is 1:3.
[0007] Compounds that convert the singlet excited state into luminescence (hereafter referred to as fluorescent compounds) No emission from the triplet excited state (phosphorescence) was observed, but emission from the singlet excited state (fluorescence) ) is observed. Therefore, the internal quantum efficiency of the light-emitting device using the fluorescent compound is The theoretical limit of the photon-to-injected carrier ratio is S * :T * =1 It is said to be 25% based on the fact that the ratio is 3:3.
[0008] On the other hand, compounds that convert the triplet excited state into luminescence (hereinafter referred to as phosphorescent compounds) are used. In some cases, light emission from the triplet excited state (phosphorescence) is observed. In addition, phosphorescent compounds exhibit intersystem crossing ( Since the transition from the singlet excited state to the triplet excited state occurs easily, the internal quantum efficiency is 7 Theoretically, it is possible to achieve 5 to 100%. In other words, the luminescence efficiency is 3 to 4 times higher than that of fluorescent compounds. For this reason, in order to realize a highly efficient light-emitting device, 2. Description of the Related Art In recent years, light-emitting devices using organic light-emitting materials have been actively developed.
[0009] When the light-emitting layer of the light-emitting element is formed using the above-mentioned phosphorescent compound, the concentration of the phosphorescent compound To suppress quenching and triplet-triplet annihilation quenching, a matrix of other compounds is used. In most cases, the phosphorescent compound is dispersed in the matrix. Compounds that are dispersed in the matrix, such as phosphorescent compounds, are called host materials. It is called material.
[0010] When a phosphorescent compound is used as a guest material, the properties required for the host material are The triplet excitation energy (energy difference between the ground state and the triplet excited state) is larger than that of the compound It is to have.
[0011] In addition, the singlet excitation energy (energy difference between the ground state and the singlet excited state) is triplet Since the triplet excitation energy is larger than the excitation energy, a material with a large triplet excitation energy has a large single Therefore, the large triplet excitation energy as described above is The substance having the above structure is also useful in a light-emitting element using a fluorescent compound as a light-emitting substance. .
[0012] Pyridinium oxide is used as a host material or an electron transport material when a phosphorescent compound is used as a guest material. Compounds having midine and the like have been studied (for example, Patent Document 1).
[0013] In addition, an example of a host material when a phosphorescent compound is used as a guest material is carbazole. Compounds combining a skeleton and a nitrogen-containing heteroaromatic ring have been disclosed (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2003-45662 A [Patent Document 2] International Publication No. 2011-046182 Summary of the Invention [Problem to be solved by the invention]
[0015] As reported in Patent Document 1 or Patent Document 2, a host material for a phosphorescent compound The development of new materials for phosphorescent compounds, or guest materials for phosphorescent compounds, is currently underway. When viewed as an element, the following aspects are considered: luminous efficiency, reliability, luminous characteristics, synthesis efficiency, and cost. There is still room for improvement, and there is a need for the development of better light-emitting devices.
[0016] In view of the above problems, one embodiment of the present invention provides a light-emitting element that has excellent heat resistance, a low driving voltage, and a long lifetime. Another embodiment of the present invention provides a light-emitting element that has excellent heat resistance and high emission efficiency. Another aspect of the present invention provides a novel heterocyclic compound. By applying ring compounds, it is possible to develop light-emitting devices with long life spans and even light-emitting devices with long life spans and high luminous efficiency. Another embodiment of the present invention is a light-emitting device and an electronic device using the light-emitting element. and a lighting device. [Means for solving the problem]
[0017] One aspect of the present invention is the synthesis of novel heterocyclic compounds having excellent heat resistance. Another embodiment of the present invention is a light-emitting element using a heterocyclic compound and having a long lifetime. In the light-emitting layer, the first organic compound, which is the novel heterocyclic compound described above, and another material are a second organic compound and a light-emitting substance that converts triplet excitation energy into light emission; By combining the first organic compound with the second organic compound, an exciplex (exciplex) is generated. The triplet excitation energy is emitted by generating an exciplex. The light-emitting element is capable of obtaining light emission from a light-emitting substance that converts the generated excitation light into The complex is a mixture of the first and second organic compounds before the exciplex formation. The S1 and T1 levels are located very close to each other compared to the difference between the S1 and T1 levels in the Therefore, the emission spectrum of the exciplex and the luminescence property that converts triplet excitation energy into light emission are The T1 level of the exciplex can be increased because the absorption spectrum of the substance can be overlapped. Increase the efficiency of energy transfer from the triplet excitation energy to the luminescent material that converts it into light. This is characterized by the fact that the light emitting efficiency of the light emitting element is improved.
[0018] That is, one embodiment of the present invention is a method for forming a pyrimidine ring and a hole between a pair of electrodes. a first organic compound that includes a ring having a transportable backbone and a second organic compound that is an aromatic amine and a layer containing a light-emitting substance that converts triplet excitation energy into light emission. The light-emitting device is a light-emitting device having one pyrimidine ring and one hole-transporting skeleton. The first organic compound containing the compound and the second organic compound which is an aromatic amine form an exciplex. The present invention is characterized in that the combination
[0019] In addition, one embodiment of the present invention is a compound having one pyrimidine ring and one hole transporting molecule between a pair of electrodes. a first organic compound containing a ring having a cyclic skeleton and having a molecular weight of 400 or more and 1200 or less; a second organic compound, which is an aromatic amine, and a photoluminescence element that converts the triplet excitation energy into light. The light-emitting element is characterized by including a layer having a pyrimidine. A ring having a hole transport skeleton and a molecular weight of 400 to 1200 The first organic compound, which is an aromatic amine, and the second organic compound, which is an aromatic amine, form an exciplex. The present invention is characterized in that the combination
[0020] In each of the above structures, the ring having a hole transport skeleton contained in the first organic compound and Examples of the ring include a carbazole ring, a dibenzothiophene ring, and a dibenzofuran ring.
[0021] In addition, since the first organic compound in each of the above structures has a high electron transporting property, it is useful as an electron transport layer, It can be used in an electron injection layer or a light emitting layer.
[0022] In each of the above structures, the ring having a hole transporting skeleton is a carbazole ring, a dibenzo It is characterized by having either a thiophene ring or a dibenzofuran ring.
[0023] Another embodiment of the present invention is a heterocyclic compound represented by the following general formula (G1): The heterocyclic compound represented by the following general formula (G1) is the first organic compound in each of the above structures. It can be used as such.
[0024] [ka]
[0025] In the formula, Ar 1 ~Ar 3each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, represents a substituted or unsubstituted phenyl group or a substituted or unsubstituted biphenyl group; R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a aryl group, or a substituted or unsubstituted aryl group. represents a phenylene group, n is 2 or 3, and Z represents oxygen or sulfur.
[0026] In the above structure, the phenylene group represented by α is an o-phenylene group, an m-phenylene group, It is characterized in that it is an nylene group or a p-phenylene group.
[0027] Another embodiment of the present invention is a heterocyclic compound represented by the following general formula (G2): The heterocyclic compound represented by the following general formula (G2) is the first organic compound in each of the above structures. It can be used as such.
[0028] [ka]
[0029] In the formula, R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or represents a substituted or unsubstituted aryl group having 6 to 13 carbon atoms. or an unsubstituted phenylene group, n is 2 or 3. Z is oxygen or sulfur. Represents yellow.
[0030] Another embodiment of the present invention is a heterocyclic compound represented by the following structural formula (100): The heterocyclic compound represented by the structural formula (100) is a compound represented by the general formula (G1) and the general formula ( G2).
[0031] [ka]
[0032] Another embodiment of the present invention is a heterocyclic compound represented by the following structural formula (101): The heterocyclic compound represented by the structural formula (101) is a compound represented by the general formula (G1) and the general formula ( G2).
[0033] [ka]
[0034] As one embodiment of the present invention, The heterocyclic compounds have excellent heat resistance, and therefore, it is possible to use these materials in light-emitting devices. In this way, a light emitting element with a long life can be formed.
[0035] Another embodiment of the present invention is a light-emitting device having a light-emitting element, as well as an electronic device having a light-emitting device. Therefore, the term "light-emitting device" in this specification includes image display devices, Also, the light emitting device has a connector, e.g. F PC (Flexible printed circuit), TCP (Tape Ca A module with a 3.5mm driver package attached, printed wiring at the end of the TCP Module with a plate or light emitting element with COG (Chip On Glass) method According to the formula, all modules on which ICs (integrated circuits) are directly mounted are also included in the light-emitting device. . Effect of the Invention
[0036] According to one embodiment of the present invention, a light-emitting element that has excellent heat resistance, a low driving voltage, and a long lifetime is provided. According to one embodiment of the present invention, a light-emitting element having excellent heat resistance and high emission efficiency can be provided. According to one embodiment of the present invention, a novel heterocyclic compound can be provided. Furthermore, by applying this new heterocyclic compound, it is possible to realize a long-lasting and heat-resistant battery. In addition, by applying this novel heterocyclic compound, It is also possible to provide a light-emitting element with a long lifetime and high emission efficiency. By using the light-emitting element described above, a light-emitting device, an electronic device, and and a lighting device. [Brief description of the drawings]
[0037] [Figure 1] FIG. 1 illustrates a concept of one embodiment of the present invention. [Diagram 2] 1A to 1C are diagrams illustrating a structure of a light-emitting element. [Diagram 3] 1A to 1C are diagrams illustrating a structure of a light-emitting element. [Figure 4] 1A to 1C are diagrams illustrating a structure of a light-emitting element. [Diagram 5] 1A and 1B are diagrams illustrating a light-emitting device. [Figure 6] 1A to 1C are diagrams illustrating electronic devices. [Figure 7] 1A to 1C are diagrams illustrating electronic devices. [Figure 8] FIG. [Figure 9] 1H-NMR chart of the heterocyclic compound shown in structural formula (100). [Figure 10] FIG. 2 shows the results of LC-MS measurement of the heterocyclic compound represented by the structural formula (100). [Figure 11] 1H-NMR chart of the heterocyclic compound shown in structural formula (101). [Figure 12]FIG. 2 shows the results of LC-MS measurement of the heterocyclic compound represented by the structural formula (101). [Figure 13] 1A to 1C are diagrams illustrating light-emitting elements. [Figure 14] FIG. 13 shows current density-luminance characteristics of Light-emitting Element 1 and Light-emitting Element 2. [Figure 15] FIG. 13 shows voltage-luminance characteristics of Light-emitting Element 1 and Light-emitting Element 2. [Figure 16] FIG. 13 shows luminance-current efficiency characteristics of Light-emitting Element 1 and Light-emitting Element 2. [Figure 17] 13 shows voltage-current efficiency characteristics of Light-emitting Element 1 and Light-emitting Element 2. [Figure 18] 1 shows the reliability of the light-emitting element 1 and the light-emitting element 2. [Figure 19] 1H-NMR chart of the heterocyclic compound shown in structural formula (112). [Figure 20] FIG. 2 shows the results of LC-MS measurement of the heterocyclic compound represented by structural formula (112). [Figure 21] FIG. 2 shows the results of LC-MS measurement of the heterocyclic compound represented by structural formula (112). [Figure 22] 1H-NMR chart of the heterocyclic compound shown in structural formula (121). [Diagram 23] FIG. 2 shows the results of LC-MS measurement of the heterocyclic compound represented by structural formula (121). [Figure 24] 13 shows current density-luminance characteristics of Light-emitting element 3 and Light-emitting element 4. FIG. [Diagram 25] 13 shows voltage-luminance characteristics of the light-emitting element 3 and the light-emitting element 4. FIG. [Figure 26] FIG. 13 shows luminance-current efficiency characteristics of Light-emitting Element 3 and Light-emitting Element 4. [Figure 27] 13 shows voltage-current efficiency characteristics of Light-emitting Element 3 and Light-emitting Element 4. [Figure 28] FIG. 13 shows the reliability of the light-emitting element 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] Hereinafter, the embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the above description, and the embodiments and details thereof are not limited to those described above without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the embodiments described below. It is not to be construed as being limited to the content.
[0039] (Embodiment 1) In this embodiment, a heterocyclic compound which is one embodiment of the present invention will be described.
[0040] The heterocyclic compound according to one embodiment of the present invention comprises one pyrimidine ring and one hole-transporting skeleton. The pyrimidine ring and the heterocyclic compound described in this embodiment are heterocyclic compounds containing a ring having a cyclic structure. The heterocyclic compound containing a ring having one hole transport skeleton is represented by the following general formula (G1): It is a heterocyclic compound having a structure as shown below.
[0041] [ka]
[0042] In general formula (G1), Ar 1 ~Ar 3 are each independently hydrogen, Any of an alkyl group, a substituted or unsubstituted phenyl group, and a substituted or unsubstituted biphenyl group. R represents 1 ~R 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a represents a substituted or unsubstituted aryl group having a carbon number of 6 to 13. represents an unsubstituted phenylene group, n represents 2 or 3, and Z represents oxygen or sulfur. The phenylene group represented by α is an o-phenylene group, an m-phenylene group, or is a p-phenylene group.
[0043] The heterocyclic compound according to one embodiment of the present invention is represented by the formula (G1) 1 ~A r 3 In the following general formula (G2), two of the groups are phenyl groups and one is hydrogen. It is more preferable to use the structure shown in the figure because it facilitates synthesis.
[0044] [ka]
[0045] In general formula (G2), R 1 ~R 3 are each independently hydrogen, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 13 carbon atoms. In addition, α represents a substituted or unsubstituted phenylene group, and n represents 2 or 3. In addition, Z is Represents oxygen or sulfur.
[0046] (α) in general formula (G1) or (G2) n (n is 2 or 3) Examples of the structures include the substituents shown in structural formulas (1-1) to (1-4). can be.
[0047] [ka]
[0048] Ar in general formula (G1) or (G2) 1 ~Ar 3 , R 1 ~R 3 The specific structure of Examples of the substituent include those shown in structural formulas (2-1) to (2-19).
[0049] [ka]
[0050] Specific examples of the heterocyclic compound that can be used in one embodiment of the present invention include compounds represented by the structural formula (100 The present invention relates to a heterocyclic compound represented by the structural formula (120). The present invention is not limited to these.
[0051] [ka]
[0052] [ka]
[0053] [ka]
[0054] [ka]
[0055] As a method for synthesizing the heterocyclic compound of one embodiment of the present invention, various reactions can be applied. For example, one of the compounds of the present invention represented by the general formula (G1) can be obtained by carrying out the reaction shown below. The heterocyclic compound according to one embodiment of the present invention can be synthesized by the method described below. The synthesis method of is not limited to the following synthesis method.
[0056] <Method for synthesizing heterocyclic compound represented by general formula (G1)> The synthesis scheme (A) of the heterocyclic compound represented by the general formula (G1) is shown below.
[0057] [ka]
[0058] In general formula (G1), Ar 1 ~Ar 3 are each independently hydrogen, Any of an alkyl group, a substituted or unsubstituted phenyl group, and a substituted or unsubstituted biphenyl group. R represents 1 ~R 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a represents a substituted or unsubstituted aryl group having a carbon number of 6 to 13. represents an unsubstituted phenylene group, n represents 2 or 3, and Z represents oxygen or sulfur. represent.
[0059] The heterocyclic compound represented by the general formula (G1) can be prepared by synthesis of a pyrimidine derivative as shown in the synthesis scheme (A). The halogenated compound (a1) of the azine derivative and dibenzothiophene or dibenzofuran, or its derivative with a boronic acid compound (a2). In the formula, X represents a halogen element. 1 and P 2 represents a substituted or unsubstituted phenylene group. In addition, l+m is n, which represents 2 or 3. In addition, B 1 is a boronic acid or boro The cyclic triol borate salts are phosphoric acid esters or cyclic triol borate salts. In addition to the lithium salt, potassium salts and sodium salts may also be used.
[0060] In addition, a boronic acid compound of a pyrimidine derivative and dibenzothiophene or dibenzofura Alternatively, a halogen compound of fluorine or a derivative thereof may be reacted.
[0061] The above-mentioned compounds (a1) and (a2) are commercially available in various types or can be synthesized. Therefore, many kinds of pyrimidine derivatives represented by general formula (G1) can be synthesized. Therefore, the heterocyclic compound according to one embodiment of the present invention can be produced in a wide variety of forms. It has the characteristic that
[0062] In the above manner, the heterocyclic compound of one embodiment of the present invention can be synthesized.
[0063] The heterocyclic compound according to one embodiment of the present invention described in this embodiment has excellent heat resistance. Therefore, by using these materials to fabricate light-emitting elements, it is possible to realize light-emitting elements with long life. In addition, the heterocyclic compound of one embodiment of the present invention is a substance with a high electron-transporting property. Therefore, it is suitable for use as a material for an electron injection layer, an electron transport layer, or a light emitting layer in a light emitting device. In addition, the heterocyclic compound according to one embodiment of the present invention can be combined with another material. By using it in a light-emitting element having a structure that forms an exciplex, it is possible to achieve a long life and high luminescence efficiency. Therefore, a light emitting element with high efficiency can be realized.
[0064] (Embodiment 2) In this embodiment, a light-emitting element using an exciplex is described. The concept of applying the heterocyclic compound according to one embodiment of the present invention described in 1 and specific examples thereof The structure of the light-emitting element will be described.
[0065] Note that the light-emitting element described in this embodiment mode is formed by sandwiching a light-emitting layer between a pair of electrodes. The light-emitting layer comprises a first organic compound, a second organic compound, and a triplet excitation energy emitting element. The organic compound is a first organic compound and a second organic compound. is a combination capable of forming an exciplex, and in the light-emitting layer, The triplet excitation energy is converted into light by the energy transfer from the luminescent material, which emits light. .
[0066] Here, the formation of an exciplex in the light-emitting layer of the light-emitting element according to one embodiment of the present invention The process is explained below. There are two possible formation processes:
[0067] The first formation process is a process in which a first organic compound (e.g., a host material) having an electron transporting property and and the second organic compound having a skeleton represented by the above general formula (G1) has a carrier. This is the process of forming an exciplex from an electron (cation or anion). In the case of the formation process, the formation of singlet excitons from the first organic compound and the second organic compound Since the formation of the light can be suppressed, a light emitting element having a long life can be realized.
[0068] The second formation process is a process in which a first organic compound (e.g., a host material) having electron transport properties and and the second organic compound having a skeleton represented by the above general formula (G1) is a singlet exciton. After the formation of the exciplex, it interacts with the other one in the ground state to form an exciplex. Once the singlet excited state of the first organic compound or the second organic compound is generated, This is quickly converted to an exciplex, so even in this case, there is no loss of singlet excitation energy or In addition, it is possible to suppress reactions from the singlet excited state, thereby realizing a light-emitting element having a long life. This can be done.
[0069] Note that in the case of a light-emitting element according to one embodiment of the present invention, either of the above two types of formation processes can be used. This also includes exciplexes formed by the combination of
[0070] In addition, in the light-emitting layer of the light-emitting element according to one embodiment of the present invention, The process of the formation of the excited complex levels and the emission of light is shown in Figure 1. As shown in FIG. 1, an exciplex 10 formed in the light-emitting layer of the light-emitting device is The S1 level and T in each of the previous substances (the first organic compound and the second organic compound) Compared to the difference in the level of 1, the S1 and T1 levels are located very close to each other. Therefore, the light emission an absorption spectrum of a luminescent material 11 that converts triplet excitation energy contained in the layer into luminescence; By increasing the overlap with the emission spectrum of the exciplex formed in the light-emitting layer, This allows the triplet excitation energy to be efficiently converted not only to the T1 energy generated in the exciplex but also to the S1 energy. The energy can be transferred to a luminescent material that converts it into light. The rate can be greatly increased.
[0071] Next, a structure of a light-emitting element which is one embodiment of the present invention will be described with reference to FIG.
[0072] As shown in FIG. 2, the light-emitting element according to one embodiment of the present invention includes a pair of electrodes (anode 101 and cathode 1 02) A first ring having one pyrimidine ring and one ring having a hole transport skeleton between the first ring and the second ring. The organic compound 105 is an aromatic amine, and the second organic compound 106 is an aromatic amine. The light-emitting layer 104 is sandwiched between the light-emitting layer 104 and the light-emitting material 107 that converts light into light. Reference numeral 104 denotes a part of a functional layer constituting the EL layer 103 that is in contact with a pair of electrodes. In addition to the light-emitting layer 104, the layer 103 includes a hole injection layer, a hole transport layer, an electrode layer, and a A electron transport layer, an electron injection layer, etc. can be appropriately selected and formed at a desired position.
[0073] The first organometallic compound having one pyrimidine ring and one ring having a hole transporting skeleton is Compound 105 is a heterocyclic compound according to one embodiment of the present invention, and is represented by the following general formula (G1): It has a structure.
[0074] [ka]
[0075] In the formula, Ar 1 ~Ar 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a substituted or unsubstituted R represents a substituted or unsubstituted phenyl group, or a substituted or unsubstituted biphenyl group. 1 ~R 3 are each independently hydrogen, an alkyl group having 1 to 4 carbon atoms, or a substituted group having 6 to 13 carbon atoms. or an unsubstituted aryl group. In addition, α represents a substituted or unsubstituted phenyl group. represents an aryl group, n is 2 or 3, and Z represents oxygen or sulfur.
[0076] Specific examples of the first organic compound represented by the general formula (G1) include the following: As this has been explained in 1, please refer to the relevant section and the explanation here will be omitted.
[0077] The second organic compound 106, which is an aromatic amine, is 4,4'-bis[N-( 1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB), N,N'-bis( 3-Methylphenyl)-N,N'-diphenyl-[1,1'-biphenyl]-4,4'- Diamine (abbreviation: TPD), 4,4'-bis[N-(spiro-9,9'-bifluorene- 2-yl)-N-phenylamino]biphenyl (abbreviation: BSPB), 4-phenyl-4' -(9-Phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-Phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation :mBPAFLP), 4-phenyl-4'-(9-phenyl-9H-carbazole-3- 4,4'-diphenyl-4''-yl)triphenylamine (abbreviation: PCBA1BP), (9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBB i1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazole-3- 4,4'-di(1-naphthyl)-4 ''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: P CBNBB), 9,9-dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazone Fluoren-2-amine (abbreviation: PCBAF), N- Phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]spiroside Aromatic amine skeleton such as PCBASF (abbreviation: PCBASF) Compounds with the same structure, such as 1,3-bis(N-carbazolyl)benzene (abbreviation: mCP), 4 ,4'-Di(N-carbazolyl)biphenyl (abbreviation: CBP), 3,6-bis(3,5- Diphenyl)phenyl)-9-phenylcarbazole (abbreviation: CzTP), 3,3'-biphenyl Carbazole skeleton such as bis(9-phenyl-9H-carbazole) (abbreviation: PCCP) Examples of the compound include compounds having the above structure.
[0078] The first organic compound 105 and the second organic compound 106 are the same as those described above. There is no restriction on the quality, and any combination that can form an exciplex may be used.
[0079] In addition, as the luminescent material 107 that converts triplet excitation energy into luminescence, a phosphorescent compound (such as an organometallic complex) or a thermally activated delayed fluorescence (TADF) material.
[0080] As the organometallic complex, for example, bis[2-(4',6'-difluorophenyl) Nyl)pyridinato-N,C 2’ ]Iridium(III) tetrakis(1-pyrazolyl)boron FIr6, bis[2-(4',6'-difluorophenyl)pyridinate] -N,C 2’ ]Iridium(III) picolinate (abbreviation: FIrpic), bis{2- [3',5'-Bis(trifluoromethyl)phenyl]pyridinato-N,C 2’}Iridescent Ir(III) picolinate (abbreviation: Ir(CF3ppy)2(pic)), bis[2- (4',6'-Difluorophenyl)pyridinato-N,C 2’ ]Iridium(III) A Cetylacetonate (abbreviation: FIracac), tris(2-phenylpyridinato)yl Ir(ppy)3, bis(2-phenylpyridinato)iridium(III) Ir(III) acetylacetonate (abbreviation: Ir(ppy)2(acac)), bis( Benzo[h]quinolinato)iridium(III) acetylacetonate (abbreviation: Ir(b zq)2(acac)), bis(2,4-diphenyl-1,3-oxazolato-N,C 2 ’ ) Iridium(III) acetylacetonate (abbreviation: Ir(dpo)2(acac) ), bis{2-[4'-(perfluorophenyl)phenyl]pyridinato-N,C2'} Iridium(III) acetylacetonate (abbreviation: Ir(p-PF-ph)2(aca c)), bis(2-phenylbenzothiazolato-N,C 2’ ) Iridium(III) acetone Ir(bt)2(acac)), bis[2-(2'-benzo[ 4,5-α]thienyl)pyridinato-N,C 3’ ]Iridium(III) acetylacetonate Ir(btp)2(acac)), bis(1-phenylisoquinolinato- N,C 2’ ) Iridium(III) acetylacetonate (abbreviation: Ir(piq)2(a cac)), (acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoline xalinato]iridium(III) (abbreviation: Ir(Fdpq)2(acac)), (acetonitrile (2,3,5-triphenylpyrazinate) bis(triphenylacetonato)iridium(III) ( Abbreviation: Ir(tppr)2(acac)), 2,3,7,8,12,13,17,18- Octaethyl-21H,23H-porphyrin platinum(II) (abbreviation: PtOEP), tri Bis(acetylacetonato)(monophenanthroline)terbium(III) (abbreviation: Tb (acac)3(Phen)), tris(1,3-diphenyl-1,3-propanedione (D)(monophenanthroline)europium(III) (abbreviation: Eu(DBM)3(Ph en)), tris[1-(2-thenoyl)-3,3,3-trifluoroacetonato](mono Nophenanthroline)europium(III) (abbreviation: Eu(TTA)3(Phen)) etc.
[0081] The light-emitting element according to one embodiment of the present invention described in this embodiment has a heat-resistant The light-emitting layer contains a heterocyclic compound having excellent optical properties, and an aromatic amine. By combining with a second organic compound, an exciplex can be formed, Increase the efficiency of energy transfer from the triplet excitation energy to the luminescent material that converts it into light. Therefore, a light-emitting element having a long life and high luminous efficiency can be realized. .
[0082] (Embodiment 3) In this embodiment, an example of a light-emitting element which is one embodiment of the present invention will be described with reference to FIG. do.
[0083] The light-emitting element shown in this embodiment has a pair of electrodes (first electrode (anode) 2) as shown in FIG. An EL layer 203 including a light-emitting layer 206 is sandwiched between a first electrode (cathode) 201 and a second electrode (cathode) 202. In addition to the light-emitting layer 206, the EL layer 203 includes a hole injection layer 204, a hole injection layer 205, and a hole injection layer 206. Alternatively, the layer may include a hole transport layer 205, an electron transport layer 207, an electron injection layer 208, etc. will be done.
[0084] In addition, the light-emitting layer 206 is the same as the light-emitting element described in the embodiment 1. The first organic compound 209 is a heterocyclic compound, and the second organic compound 208 is an aromatic amine. and a light-emitting material 211 that converts triplet excitation energy into light emission. The first organic compound 209, the second organic compound 210, and the triplet excited electrons are The luminescent material 211 that converts energy into luminescence is the same as that shown in the first or second embodiment. Since the same material as that used in the embodiment can be used, the description thereof will be omitted.
[0085] The first electrode (anode) 201 and the second electrode (cathode) 202 are made of a metal, an alloy, an electrically conductive material, or Conductive compounds and mixtures thereof can be used. Indium-tin oxide (ITO), silicon or silicon oxide Indium oxide-tin oxide and indium oxide-zinc oxide (Indium Zi nc Oxide), indium oxide containing tungsten oxide and zinc oxide, gold (A u), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo) Mo, Fe, Co, Cu, Pd, Ti In addition to Ti, elements in the first or second group of the periodic table, namely lithium (L i) and cesium (Cs), as well as magnesium (Mg), calcium ( Alkaline earth metals such as Ca, Strontium (Sr), and alloys containing these metals (Mg Rare earth metals such as Ag, AlLi), europium (Eu), ytterbium (Yb) and The first electrode (anode) may be a cathode material, an alloy containing the above-mentioned, or graphene. The first electrode (cathode) 201 and the second electrode (cathode) 202 are formed by, for example, sputtering or deposition (vacuum The thin film can be formed by a method such as vapor deposition.
[0086] The hole-injection layer 204 and the hole-transport layer 205 may be formed of a material having a high hole-transporting property, for example. For example, 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation :NPB or α-NPD) and N,N'-bis(3-methylphenyl)-N,N'-diphenyl Phenyl-[1,1'-biphenyl]-4,4'-diamine (abbreviation: TPD), 4,4', 4''-Tris(carbazol-9-yl)triphenylamine (abbreviation: TCTA), 4 ,4',4''-Tris(N,N-diphenylamino)triphenylamine (abbreviation: TD ATA), 4,4',4''-tris[N-(3-methylphenyl)-N-phenylamine N-(spiro-9, 9'-Bifluoren-2-yl)-N-phenylamino]biphenyl (abbreviation: BSPB) Aromatic amine compounds such as 3-[N-(9-phenylcarbazol-3-yl)-N- Phenylamino]-9-phenylcarbazole (abbreviation: PCzPCA1), 3,6-bis [N-(9-phenylcarbazol-3-yl)-N-phenylamino]-9-phenyl Carbazole (abbreviation: PCzPCA2), 3-[N-(1-naphthyl)-N-(9-phenyl PCzPC Other examples include 4,4'-di(N-carbazolyl)biphenyl (abbreviation: CBP), 1,3,5-tris[4-(N-carbazolyl)phenyl]benzene (abbreviation: TCPB), 9-[4-(10-phenyl-9-anthracenyl)phenyl]-9H-ca Carbazole derivatives such as carbazole (abbreviation: CzPA) can be used. The substances mentioned in are mainly -6 cm 2 A material that has a hole mobility of at least / Vs. Any other substance may be used as long as it has a higher hole transporting property than an electron transporting property.
[0087] In addition, poly(N-vinylcarbazole) (abbreviation: PVK), poly(4-vinyltriflate) phenylamine) (abbreviation: PVTPA), poly[N-(4-{N'-[4-(4-diphenyl phenyl-N'-phenylamino}phenyl)methacrylamide (abbreviation: PTPDMA), poly[N,N'-bis(4-butylphenyl)-N,N'-bi Poly(phenyl)benzidine (abbreviation: Poly-TPD) and other polymer compounds are used. It is also possible.
[0088] In addition, examples of acceptor substances that can be used in the hole injection layer 204 include transition metals, Examples of the oxides include oxides of metals belonging to groups 4 to 8 of the periodic table. Specifically, molybdenum oxide is particularly preferred.
[0089] The light-emitting layer 206 is as described above, and includes a first organic compound 209 having an electron transporting property and A second organic compound 210 having a skeleton represented by general formula (G1) (a triplet excitation The light-emitting device may further include a luminescent material that converts photovoltaic energy into light.
[0090] The electron transport layer 207 is a layer containing a substance with a high electron transporting property. Alq3, tris(4-methyl-8-quinolinolato)aluminum (abbreviation: Almq3) , Bis(10-hydroxybenzo[h]quinolinato)beryllium (abbreviation: BeBq2), BAlq, Zn(BOX)2, bis[2-(2-hydroxyphenyl)benzothiazol ] zinc (abbreviation: Zn(BTZ)2) and other metal complexes can be used. 4-biphenylyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazide PBD, 1,3-bis[5-(p-tert-butylphenyl)-1, 3,4-Oxadiazol-2-yl]benzene (abbreviation: OXD-7), 3-(4'-t ert-butylphenyl)-4-phenyl-5-(4''-biphenyl)-1,2,4- Triazole (abbreviation: TAZ), 3-(4-tert-butylphenyl)-4-(4-ethylphenyl) pE(phenyl)-5-(4-biphenylyl)-1,2,4-triazole tTAZ), Bathophenanthroline (abbreviation: BPhen), Bathocuproine (abbreviation: B CP), 4,4'-bis(5-methylbenzoxazol-2-yl)stilbene (abbreviation Heteroaromatic compounds such as poly(2,5-pyridyl) and poly(2,5-pyridyl) are also useful. Poly[(9,9-dihexylfluorene-2,7-diyne] (abbreviation: PPy) poly[(9,9- Dioctylfluorene-2,7-diyl)-co-(2,2'-bipyridine-6,6'- Polymer compounds such as PF-BPy (abbreviation: PF-BPy) can also be used. The substances mentioned are mainly 10 -6 cm 2 / Vs or more. Any substance other than the above may be used for the electron transport layer 207 as long as it has a higher electron transporting property than the hole transporting property. This is also fine.
[0091] In addition, the electron transport layer 207 may be a single layer or may be a laminate of two or more layers of the above-mentioned materials. It may also be layered.
[0092] The electron injection layer 208 is a layer containing a substance with high electron injection properties. Lithium fluoride (LiF), Cesium fluoride (CsF), Calcium fluoride (CaF2) , lithium oxide (LiOx), etc., alkaline metals, alkaline earth metals, or the like Also, rare earth compounds such as erbium fluoride (ErF3) can be used. Metal compounds can be used. In addition, the above-mentioned material constituting the electron transport layer 207 can be used. You can also be there.
[0093] Alternatively, the electron injection layer 208 may be formed by mixing an organic compound and an electron donor. Composite materials may also be used. Such composite materials are made by adding electrons to organic compounds by electron donors. In this case, the organic compound is In particular, the material is preferably one that is excellent in transporting the generated electrons. The material constituting the electron transport layer 207 (metal complex, heteroaromatic compound, etc.) can be used. The electron donor may be any substance that exhibits electron donating properties to organic compounds. Specifically, alkali metals, alkaline earth metals and rare earth metals are preferred, and lithium, cesium, etc. Examples of the elements include aluminum, magnesium, calcium, erbium, and ytterbium. Alkali metal oxides and alkaline earth metal oxides are preferred, and lithium oxide, calcium oxide, Examples of the cations include barium oxide and barium phosphate. In addition, Lewis bases such as magnesium oxide are used. It is also possible to use organic compounds such as tetrathiafulvalene (TTF). It is also possible.
[0094] The hole injection layer 204, the hole transport layer 205, the light emitting layer 206, and the electron transport layer 20 7, the electron injection layer 208 is formed by a deposition method (including a vacuum deposition method), an inkjet method, The layer can be formed by a coating method or the like.
[0095] The light emitted from the light emitting layer 206 of the above-mentioned light emitting device is generated by the first electrode 201 and the second electrode 202. The electric current is taken out through one or both of the electrodes 202. Either or both of the first electrode 201 and the second electrode 202 in The electrode has the following structure.
[0096] In this embodiment, the heterocyclic compound of one embodiment of the present invention is used in the light-emitting layer of the light-emitting element. An exciplex is generated from the applied first organic compound 209 and second organic compound 210. The triplet excitation energy is converted from the generated exciplex into a luminescent material 211 that emits light. The efficiency of energy transfer can be improved, resulting in a long life and highly efficient light-emitting diode. Optical elements can be realized.
[0097] Note that the light-emitting element described in this embodiment is one embodiment of the present invention, and in particular, Therefore, by applying the configuration shown in this embodiment, It is possible to manufacture a light-emitting device of a switch type or an active matrix type. are all included in the present invention.
[0098] In the case of an active matrix type light emitting device, the structure of the TFT is not particularly limited. For example, a staggered or inverted staggered TFT can be used as appropriate. The driver circuit formed on the FT substrate may consist of N-type and P-type TFTs. Alternatively, it may be composed of only one of N-type TFTs or P-type TFTs. Furthermore, there is no particular limitation on the crystallinity of the semiconductor film used in the TFT. An amorphous semiconductor film, a crystalline semiconductor film, an oxide semiconductor film, or the like can be used.
[0099] Note that the structure described in this embodiment mode may be used in appropriate combination with structures described in other embodiments. It is possible to do so.
[0100] (Embodiment 4) In this embodiment, as one embodiment of the present invention, a structure having a plurality of EL layers sandwiching a charge generating layer is described. A light emitting device having this structure (hereinafter referred to as a tandem type light emitting device) will be described.
[0101] The light-emitting element shown in this embodiment has a pair of electrodes (first electrode 30) as shown in FIG. A plurality of EL layers (first EL layer 302(1), second EL layer 302(2), and second EL layer 304) are disposed between the first and second electrodes 302(3), 302(4), 302(5), 302(6), 302(7), 302(8), 302(9), 302(10), 302(11), 302(12), 302(13 This is a tandem type light emitting device having an L layer 302(2).
[0102] In this embodiment, the first electrode 301 is an electrode that functions as an anode, and the second The electrode 304 functions as a cathode. The structure of the EL layer 304 may be the same as that of the first embodiment. The first EL layer 302(1) and the second EL layer 302(2) are the same as those in the first embodiment or the second embodiment. The EL layer may have a similar structure to that shown in 2, but either one may have a similar structure. That is, the first EL layer 302(1) and the second EL layer 302(2) have the same structure. The configuration may be the same as that of the first or second embodiment. can be applied.
[0103] In addition, between the multiple EL layers (the first EL layer 302(1) and the second EL layer 302(2)), The charge generating layer 305 is provided between the first electrode 301 and the second electrode 302. When a voltage is applied to the electrode 304, electrons are injected into one EL layer and positive charge is injected into the other EL layer. In the present embodiment, the first electrode 301 is connected to the second electrode 302. When a voltage is applied so that the potential becomes higher than that of the charge generating layer 304, the charge generating layer 305 generates a charge to the first EL layer 305. Electrons are injected into 302(1) and holes are injected into the second EL layer 302(2).
[0104] From the viewpoint of light extraction efficiency, the charge generating layer 305 is transparent to visible light. (Specifically, the visible light transmittance of the charge generating layer 305 is preferably 40% or more.) In addition, the charge generating layer 305 has a lower conductivity than the first electrode 301 and the second electrode 304. It also works as a percentage.
[0105] The charge generation layer 305 is made of an organic compound with high hole transport properties to which an electron acceptor is added. Even in the case of a structure in which an electron donor is added, the electron donor is added to an organic compound with high electron transport properties. Alternatively, both of these configurations may be laminated.
[0106] In the case where an electron acceptor is added to an organic compound having a high hole transporting property, Examples of organic compounds with high transportability include NPB, TPD, TDATA, and MTDATA. , 4,4'-bis[N-(spiro-9,9'-bifluoren-2-yl)-N-phenyl Aromatic amine compounds such as bisaminobiphenyl (abbreviation: BSPB) can be used. The substances mentioned here are mainly -6 cm 2 / Vs or more. However, if an organic compound has a higher hole transporting property than an electron transporting property, a substance other than the above may be used. That's fine.
[0107] In addition, 7,7,8,8-tetracyano-2,3,5,6-tetracyanophenylacetate can be used as an electron acceptor. Examples include fluoroquinodimethane (abbreviation: F4-TCNQ) and chloranil. Further, transition metal oxides can be used. Specifically, vanadium oxide, niobium oxide, etc. , Tantalum oxide, Chromium oxide, Molybdenum oxide, Tungsten oxide, Manganese oxide, Oxide Rhenium is preferred because of its high electron-accepting property. In particular, molybdenum oxide is stable even in the atmosphere. It is preferable because it is stable, has low hygroscopicity, and is easy to handle.
[0108] On the other hand, in the case where an electron donor is added to an organic compound having high electron transport properties, Examples of organic compounds with high electron transport properties include Alq, Almq3, BeBq2, and B Metal complexes having a quinoline or benzoquinoline skeleton, such as Alq, can be used. In addition, oxazole-based compounds such as Zn(BOX)2 and Zn(BTZ)2, Metal complexes having azole-based ligands can also be used. However, PBD, OXD-7, TAZ, BPhen, BCP, etc. can also be used. The substances mentioned in are mainly -6 cm 2 / Vs or higher. Any organic compound having a higher electron transporting property than a hole transporting property may be used. stomach.
[0109] The electron donor may be an alkali metal, an alkaline earth metal, a rare earth metal, or or metals belonging to Group 13 of the periodic table and their oxides and carbonates. Specifically, lithium (Li), cesium (Cs), magnesium (Mg), Calcium (Ca), Ytterbium (Yb), Indium (In), Lithium oxide, Carbonate It is preferable to use cesium, etc. Also, organic compounds such as tetrathianaphthacene may be used as the electron donor.
[0110] In addition, the charge generating layer 305 is formed using the above-mentioned material, and the EL layer is laminated. In this case, the increase in the driving voltage can be suppressed.
[0111] In this embodiment mode, a light-emitting element having two EL layers has been described. As described above, the same can be said for a light-emitting device having n (n is 3 or more) stacked EL layers. As in the light-emitting device according to the present embodiment, a compound semiconductor device is provided between a pair of electrodes. When the device has multiple EL layers, the current density can be improved by disposing a charge generating layer between the EL layers. It is possible to emit light in a high brightness range while keeping the current density low. In addition, when applied to lighting, the voltage drop due to the resistance of the electrode material can be reduced. The bottom can be made small, enabling uniform light emission over a large area. A light emitting device with low power consumption can be realized.
[0112] In addition, by making the emission color of each EL layer different, the light-emitting element as a whole can be For example, in a light-emitting device having two EL layers, the first By making the emission color of the first EL layer and the emission color of the second EL layer complementary to each other, It is also possible to obtain a light-emitting element that emits white light as a whole. In other words, the color that becomes achromatic when it is combined with the color that is complementary is called the color of the substance that emits the color. When the resulting light is mixed, white light can be obtained.
[0113] The same applies to a light-emitting element having three EL layers. For example, The emission color of the first EL layer is red, the emission color of the second EL layer is green, and the emission color of the third EL layer is blue. In this case, the light emitting element as a whole can emit white light.
[0114] In addition to the structure in which the EL layer is laminated via the charge generating layer as described in this embodiment, By setting the distance between the electrodes (the first electrode 301 and the second electrode 304) to a desired value, This is a light-emitting element that has a micro-optical resonator (microcavity) structure that utilizes the resonance effect of light. It's good as a child too.
[0115] Note that the structure described in this embodiment mode may be used in appropriate combination with structures described in other embodiments. There can be.
[0116] (Embodiment 5) In this embodiment, a light-emitting device including a light-emitting element which is one embodiment of the present invention will be described. .
[0117] As the light emitting element, the light emitting elements described in the other embodiments can be applied. In addition, the light-emitting device may be a passive matrix type light-emitting device or an active matrix type light-emitting device. Any type of light emitting device may be used, but in this embodiment, an active matrix type light emitting device is used. This will be explained with reference to FIG. 5.
[0118] 5(A) is a top view showing the light emitting device, and FIG. 5(B) is a top view showing the light emitting device along the dashed line A- 1 is a cross-sectional view taken along line A' of an active matrix light-emitting device according to the present embodiment. A pixel section 502 and a driving circuit section (source line driving circuit) 50 are provided on an element substrate 501. 3 and driver circuit sections (gate line driver circuits) 504a and 504b. The driver circuit portion 503 and the driver circuits 504a and 504b are sealed by a sealant 505. It is sealed between the element substrate 501 and a sealing substrate 506 .
[0119] In addition, on the element substrate 501, a driving circuit section 503, and driving circuit sections 504a and 504b are provided. An external signal (e.g. video signal, clock signal, start signal, or reset signal) A wiring 507 is provided for connecting an external input terminal for transmitting a signal or potential. Here, we set FPC (flexible printed circuit) 508 as the external input terminal. This is an example of a FPC. Note that only the FPC is shown here, but the FPC has a plug. A printed wiring board (PWB) may be attached. This includes not only the light emitting device itself, but also the state in which the FPC or PWB is attached to it. It shall be so.
[0120] Next, the cross-sectional structure will be described with reference to FIG. A driver circuit portion 503 which is a source line driver circuit is formed in the pixel portion. 5, a pixel portion 502 is shown.
[0121] The driving circuit section 503 is a combination of an n-channel TFT 509 and a p-channel TFT 510. The circuit forming the driver circuit section is shown in FIG. It may be formed of various CMOS circuits, PMOS circuits, or NMOS circuits. In the embodiment, a driver integrated type in which a driving circuit is formed on a substrate is shown, but this is not necessarily required. It is not necessary, and the driving circuit can be formed externally instead of on the substrate.
[0122] The pixel section 502 includes a switching TFT 511, a current control TFT 512, and a current A first TFT 512 electrically connected to the wiring (source electrode or drain electrode) of the control TFT 512 The first electrode (anode) 513 is formed of a plurality of pixels. An insulator 514 is formed covering the end of the substrate 13. Here, a positive photosensitive acrylic is used. It is formed by using a resin.
[0123] In order to improve the coverage of the film to be laminated on the upper layer, the upper end of the insulator 514 It is preferable that a curved surface having a curvature is formed at the upper or lower end. When a positive photosensitive acrylic resin is used as the material of the insulating material 514, the upper end of the insulating material 514 It is preferable that the insulating layer has a curved surface with a radius of curvature (0.2 μm to 3 μm). Either a negative photosensitive resin or a positive photosensitive resin can be used as the material 514. It is possible to use not only organic compounds but also inorganic compounds such as silicon oxide and silicon oxynitride. Both of these can be used.
[0124] An EL layer 515 and a second electrode (cathode) 516 are laminated on a first electrode (anode) 513. The EL layer 515 is formed of at least the EL layer 517 of the embodiment. The EL layer 515 includes the light-emitting layer described in 1. In addition to the light-emitting layer, a hole injection layer, A hole transport layer, an electron transport layer, an electron injection layer, a charge generation layer, and the like can be appropriately provided.
[0125] Also, the first electrode (anode) 513, the EL layer 515, and the second electrode (cathode) 516 are made of As the material, the material shown in the embodiment mode 2 can be used. However, the second electrode (cathode) 516 is electrically connected to the FPC 508 which is an external input terminal. It has been done.
[0126] In addition, although only one light-emitting element 517 is shown in the cross-sectional view shown in FIG. In the pixel section 502, a plurality of light emitting elements are arranged in a matrix. 02, selectively forming light-emitting elements that can emit three types of light (R, G, B), It is possible to form a light-emitting device capable of full color display. By combining these, a light emitting device capable of full color display may be obtained.
[0127] Furthermore, a sealing substrate 506 is bonded to the element substrate 501 with a sealant 505. The light is emitted into a space 518 surrounded by the element substrate 501, the sealing substrate 506, and the sealant 505. The structure is provided with an element 517. The space 518 is filled with an inert gas (such as nitrogen, etc.). In addition to the case where the cavity is filled with a gas such as argon, the cavity may also be filled with a sealing material 505. .
[0128] It is preferable to use an epoxy resin for the sealing material 505. It is preferable that the sealing substrate 506 is made of a material that is as impermeable to moisture and oxygen as possible. In addition to glass and quartz substrates, FRP (Fiberglass-Reinforced Plastics) is also used as a material for unforced Plastics), PVF (Polyvinyl fluoride), Polyester Alternatively, a plastic substrate made of acrylic or the like can be used.
[0129] In this manner, an active matrix light emitting device can be obtained.
[0130] Note that the structure described in this embodiment mode may be used in appropriate combination with structures described in other embodiment modes. There can be.
[0131] (Embodiment 6) In this embodiment, a light-emitting device manufactured using a light-emitting element according to one embodiment of the present invention is used. Examples of various electronic devices completed using this method will be described with reference to FIGS. 6 and 7.
[0132] As an example of an electronic device to which a light-emitting device is applied, a television set (a television, (also called TV receivers), computer monitors, digital cameras, digital video digital cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), Examples include portable game machines, personal digital assistants, audio playback devices, and large game machines such as pachinko machines. Specific examples of these electronic devices are shown in Figure 6.
[0133] FIG. 6A shows an example of a television device. The television device 7100 includes: A display unit 7103 is built into the housing 7101. The display unit 7103 displays images. It is possible to use a light-emitting device in the display portion 7103. 7 shows a configuration in which a housing 7101 is supported by a stand 7105.
[0134] The television device 7100 can be operated using an operation switch provided on the housing 7101 or a separate remote control. This can be done by using the remote control operation device 7110. The channel and volume can be controlled by the 7109, and the display 7103 shows In addition, the remote control unit 7110 can be used to control the video. A display unit 7107 for displaying information output from the device 7110 may be provided.
[0135] The television device 7100 includes a receiver, a modem, and the like. It is possible to receive general television broadcasts, and furthermore to receive them by wired or wireless connection via a modem. By connecting to a communication network, it is possible to communicate in one direction (from sender to receiver) or two directions ( It is also possible to communicate information between a sender and a receiver, or between receivers themselves.
[0136] FIG. 6B shows a computer, which includes a main body 7201, a housing 7202, a display unit 7203, and a keyboard. keyboard 7204, external connection port 7205, pointing device 7206, etc. Note that the computer is manufactured by using a light-emitting device for the display portion 7203. .
[0137] FIG. 6C shows a portable game machine that is composed of two housings, a housing 7301 and a housing 7302. The housing 7301 is connected to the display unit 7302 by a connecting portion 7303 so as to be openable and closable. A display unit 7305 is incorporated in the housing 7302. The portable gaming machine shown in FIG. 6(C) also includes a speaker unit 7306 and a recording medium insertion unit 7307. , LED lamp 7308, input means (operation keys 7309, connection terminal 7310, sensor 73 11 (force, displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical Chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration , odor or infrared measuring function), microphone 7312) etc. Of course, the configuration of the portable gaming machine is not limited to the above, and at least the display unit 73 04 and the display portion 7305, or either one of them may use a light-emitting device. The portable gaming machine shown in FIG. The function of reading out the programs or data recorded on the media and displaying them on the display unit, and other It has a function to share information with the portable game machine by wireless communication. The functions of the portable gaming machine are not limited to these, and the portable gaming machine may have a variety of functions.
[0138] FIG. 6D shows an example of a mobile phone. A mobile phone 7400 includes a housing 7401. In addition to the display unit 7402, operation buttons 7403, an external connection port 7404, The mobile phone 7400 is equipped with a speaker 7405, a microphone 7406, and the like. The device is used for the display portion 7402 .
[0139] In a mobile phone 7400 shown in FIG. 6D, information can be displayed by touching a display portion 7402 with a finger or the like. You can also make calls, write emails, and perform other operations. This can be done by touching the display portion 7402 with a finger or the like.
[0140] The screen of the display unit 7402 has three main modes. The first is a mode that mainly displays images. The first mode is a display mode, the second is an input mode for inputting information such as characters, and the third mode is a display mode. This is a display + input mode that combines the display mode and the input mode.
[0141] For example, when making a call or composing an e-mail, the display unit 7402 is used for inputting characters. The main input mode is the character input mode, and the input operation of the characters displayed on the screen can be performed. In this case, it is preferable to display a keyboard or number buttons on most of the screen of the display portion 7402. I wish.
[0142] In addition, a sensor for detecting tilt, such as a gyro or an acceleration sensor, is installed inside the mobile phone 7400. By providing a detection device having the above, the orientation of the mobile phone 7400 (portrait or landscape) can be determined, The screen display on the display portion 7402 can be automatically switched.
[0143] The screen mode can be changed by touching the display portion 7402 or by operating the housing 7401. The type of image displayed on the display unit 7402 can be selected by operating the operation button 7403. For example, the image signal to be displayed on the display unit may be changed by If the data is text data, the mode switches to input mode.
[0144] In the input mode, the optical sensor of the display unit 7402 detects a signal and displays the If there is no input by touch operation on the display unit 7402 for a certain period of time, the screen mode is changed to the input mode. Alternatively, the display mode may be switched from the display mode to the display mode.
[0145] The display unit 7402 can also function as an image sensor. By touching 402 with a palm or a finger and capturing an image of a palm print, fingerprint, or the like, personal authentication can be performed. In addition, a backlight that emits near-infrared light to the display unit or a sensing light that emits near-infrared light By using a source, it is also possible to image finger veins, palm veins, etc.
[0146] Figures 7(A) and 7(B) show tablet terminals that can be folded in half. Figure 7(A) shows In the open state, the tablet terminal includes a housing 9630, a display unit 9631a, and a display unit 96 31b, a display mode changeover switch 9034, a power switch 9035, a power saving mode changeover switch The switch 9036, the fastener 9033, and the operation switch 9038 are included. The tablet terminal has a light emitting device in one or both of the display portions 9631a and 9631b. It is produced by using
[0147] A part of the display unit 9631a can be used as a touch panel area 9632a. By touching the operation keys 9637 displayed on the display unit 96, data can be input. In 31a, as an example, half of the area has a display function only, and the other half The display unit 96 has a touch panel function, but is not limited to this. The entire area of the display unit 931a may have a touch panel function. The entire surface of 631a is made to display keyboard buttons to serve as a touch panel, and the display section 9631b is made to display It can be used as a display screen.
[0148] In addition, in the display unit 9631b, as in the display unit 9631a, The part of the touch panel can be the area 9632b of the touch panel. Touch the area where the mode display switch button 9639 is displayed with your finger or a stylus. A keyboard button can be displayed on the display portion 9631b.
[0149] In addition, the touch panel area 9632a and the touch panel area 9632b are simultaneously You can also use touch input.
[0150] A display mode changeover switch 9034 is used to change the display orientation, such as portrait or landscape. You can switch between black and white and color display. The switch 9036 is a switch that turns on and off when the tablet terminal is in use and is detected by a light sensor built into the tablet terminal. The brightness of the display can be optimized according to the amount of light. In addition to sensors, other detection devices such as gyros, acceleration sensors, etc. that detect tilt may be incorporated.
[0151] FIG. 7A shows an example in which the display area of the display portion 9631b is the same as that of the display portion 9631a. However, there is no particular limitation, and one size may be different from the other size. For example, one display panel may have a higher resolution than the other. It is also possible to use the following.
[0152] FIG. 7B shows the tablet terminal in a closed state. The tablet terminal includes a housing 9630 and a solar cell 96 33, a charge / discharge control circuit 9634, a battery 9635, and a DCDC converter 9636 In addition, in FIG. 7B, a battery 9635 is used as an example of the charge and discharge control circuit 9634. A configuration having a DC-DC converter 9636 is shown.
[0153] In addition, since the tablet device can be folded in half, the case 9630 can be folded when not in use. Therefore, the display portions 9631a and 9631b can be protected. This makes it possible to provide a tablet device that is highly durable and reliable even when used for a long period of time.
[0154] In addition, the tablet terminals shown in Figs. 7(A) and 7(B) can display various information. Functions that display (still images, videos, text images, etc.), calendars, dates, or times, etc. A function to display information on the display unit, and a touch input function to operate or edit information displayed on the display unit Functions such as the ability to control processing using various software (programs) can be done.
[0155] The solar cell 9633 attached to the surface of the tablet device supplies power to the touch panel. The solar cell 9633 can supply the light to a display unit, a video signal processor, or the like. , which can be provided on one or both sides of the housing 9630, and can efficiently charge the battery 9635. The battery 9635 may be a lithium-ion battery. The use of a pond has the advantage of making it possible to reduce the size.
[0156] The configuration and operation of the charge / discharge control circuit 9634 shown in FIG. A block diagram is shown and explained in FIG. 7(C). , DC-DC converter 9636, converter 9638, switches SW1 to SW3, display The figure shows the part 9631, the battery 9635, the DCDC converter 9636, The inverter 9638 and the switches SW1 to SW3 are connected to the charge / discharge control circuit 96 shown in FIG. This corresponds to 34.
[0157] First, an example of operation in which power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell 9633 becomes the voltage for charging the battery 9635. The voltage is increased or decreased by the DC-DC converter 9636. When power is used from the Solar Cell 9633, switch SW1 is turned on and the The inverter 9638 increases or decreases the voltage to the voltage required for the display unit 9631. When the display unit 9631 is not to be displayed, the switch SW1 is turned off and the switch S The configuration may be such that W2 is turned on to charge the battery 9635.
[0158] The solar cell 9633 is shown as an example of a power generating means, but is not limited thereto. Other power generation methods such as piezoelectric elements and thermoelectric conversion elements (Peltier elements) For example, the battery 9635 may be charged. A non-contact power transmission module that receives and charges, or a structure that combines other charging methods It may also be composed of.
[0159] In addition, if the display unit described in the above embodiment is provided, the electronic device shown in FIG. Needless to say, the present invention is not limited to the above.
[0160] In the above manner, an electronic device can be obtained by using the light-emitting device which is one embodiment of the present invention. The range of applications for light-emitting devices is extremely wide, and they can be used in electronic devices in a wide range of fields. It is.
[0161] Note that the structure described in this embodiment mode may be used in appropriate combination with structures described in other embodiments. There can be.
[0162] (Embodiment 7) In this embodiment, a lighting device including a light-emitting device which is one embodiment of the present invention is used. An example of this will be described with reference to FIG.
[0163] FIG. 8 shows an example in which the light emitting device is used as an indoor lighting device 8001. It is also possible to make the surface area larger, so a large-area lighting device can be formed. By using a housing having such a structure, it is possible to form a lighting device 8002 having a curved light-emitting area. The light-emitting element included in the light-emitting device shown in this embodiment mode has a thin film shape, and the design of the housing can be changed. Therefore, lighting devices with various elaborate designs can be created. Furthermore, a large lighting device 8003 may be provided on the wall of the room.
[0164] In addition, by using a light-emitting device on the surface of a table, a lighting device that also functions as a table can be provided. The lighting device 8004 can be used as a lighting device. This makes it possible to provide a lighting device that also functions as furniture.
[0165] As described above, various lighting devices using the light-emitting device can be obtained. The device is considered to be included in one aspect of the present invention.
[0166] The structure described in this embodiment may be used in appropriate combination with structures described in other embodiments. There can be. EXAMPLES
[0167] <Synthesis Example 1> In this example, a complex compound represented by the structural formula (100) of the embodiment 1 according to the present invention is Ring compound, 4-[3'-(4-dibenzothienyl)-1,1'-biphenyl-3-yl] -2,6-diphenylpyrimidine (abbreviation: 2,6Ph-4mDBTBPPm-II) The synthesis method of 2,6Ph-4mDBTBPPm-II (abbreviation) is as follows: is shown below.
[0168] [ka]
[0169] Step 1: Synthesis of 4-(3-bromophenyl)-2,6-diphenylpyrimidine The synthesis scheme of 4-(3-bromophenyl)-2,6-diphenylpyrimidine is shown below (B- 1).
[0170] [ka]
[0171] Add 18.5 g (100.0 mmol) of 3-bromobenzaldehyde to a 500 mL three-neck flask. l), acetophenone 12.0g (100.0mmol) was added, and the mixture was replaced with nitrogen and ethanol was added. To this mixture was added 6.0 g (111.0 mmol) of sodium methoxide. A solution of l) suspended in 100 mL of ethanol was added dropwise and stirred at room temperature for 22 hours. After stirring for 1 hour, 15.6 g (100.0 mmol) of benzamidine hydrochloride and sodium hydroxide were added. 8.0 g (200.0 mmol) of ethanol was added and stirred at 70°C for 3 hours. After stirring, the mixture was filtered. The residue was added with water and ultrasonically washed. The solid was collected by suction filtration, and the white solid was 14.4 g. g, yield 38.0%.
[0172] <Step 2: Synthesis of 2,6Ph-4mDBTBPPm-II (abbreviation)> The synthesis scheme of 2,6Ph-4mDBTBPPm-II (abbreviation) is shown in (B-2).
[0173] [ka]
[0174] Add 4-(3-bromophenyl)-2,6-diphenylpyrimidinium to a 500 mL three-neck flask. 7.75g (20.0mmol), 3-(dibenzothiophen-4-yl)phenyl 7.60g (25.0mmol) of uronic acid, 608.7mM of tris(o-tolyl)phosphine g (2.0 mmol) was added to the mixture, and 155 mL of toluene, 20 mL of ethanol, 25 mL of 2M aqueous potassium carbonate was added. The mixture was degassed under reduced pressure with stirring. Then, 224.5 mg (1.0 mmol) of palladium (II) acetate was added and the mixture was stirred for 80 The mixture was reacted at 0.5 °C for 2.5 hours with stirring. After the reaction, 1300 mL of toluene was added and separated. The extract was extracted with toluene, and the organic layer was washed with saturated saline and then with magnesium sulfate. After drying, the mixture was gravity filtered, then filtered through Celite and alumina. The filtrate was concentrated and recrystallized from toluene to give 9.64 g of a white solid in 85.1% yield. Ta.
[0175] The nuclear magnetic resonance spectroscopy of the compound obtained by the above synthesis method ( 1 The results of the analysis using H-NMR are shown below. As shown below. 1 The H-NMR chart is shown in FIG. 9. From the results, it is clear that the compound of the above structural formula (1 00) is a heterocyclic compound according to one embodiment of the present invention. -II (abbreviation) was obtained.
[0176] 1 H NMR(CDCl3,500MHz):δ=7.46-7.61(m, 10H) , 7.66-7.70(dt, J=2.5Hz, 7.8Hz, 2H), 7.78-7.8 1(t, J=7.7Hz, 3H), 7.87-7.88(d, J=8.0Hz, 1H), 8.01(s, 1H), 8.14-8.15(t, J=1.7Hz, 1H), 8.20- 8.23(m, 2H), 8.31-8.33(dd, J=2.3Hz, 7.4Hz, 3H ), 8.60-8.61(t, J=1.7Hz, 1H), 8.74-8.63(m, 2H ).
[0177] Next, 2,6Ph-4mDBTBPPm-II (abbreviation) obtained in this example was subjected to liquid chromatography. Liquid Chromatography Mass Spectrometry The results were analyzed by LC / MS (liquid crystal spectrometry).
[0178] LC / MS analysis was performed using Waters Acquity UPLC and Waters The analysis was performed using a Xevo G2 Tof MS manufactured by Eppendorf.
[0179] In the MS analysis, electrospray ionization was used. The capillary voltage was set at 3 The voltage was 0.0 kV, the sample cone voltage was 30 V, and detection was performed in positive mode. The components ionized under the above conditions are collided with argon gas in a collision cell. The energy of the collision of argon (collision) was The electron energy was set to 70 eV. The mass range of the measurement was m / z = 100 to 1200. It was decided.
[0180] The measurement results are shown in FIG. 10. From the results in FIG. 10, one of the compounds of the present invention represented by the structural formula (100) The heterocyclic compound 2,6Ph-4mDBTBPPm-II (abbreviation) is mainly Around m / z=361, around m / z=345, around m / z=258, around m / z=128, It was found that product ions were detected at m / z = 104. The results shown in Fig. 0 are characteristic results derived from 2,6Ph-4mDBTBPPm-II (abbreviation). Since this shows the effect, the 2,6Ph-4mDBTBPPm-I contained in the mixture This is important data for identifying I (abbreviation).
[0181] In addition, the CC bond next to the N atom of the pyrimidine ring breaks and the fragment containing the N atom Because the charge remains, the areas around m / z=361, m / z=128, and m / z=104 are In each case, the C—C bond next to the N atom of the pyrimidine ring of the compound of structural formula (100) is broken. It is useful because it is assumed that information on the At m / z=258, there are two benzothiophene rings and two benzene rings. It can be assumed that each of these product ions contains one benzene ring, which is one aspect of the present invention. The heterocyclic compound, 2,6Ph-4mDBTBPPm-II (abbreviation), is a dibenzothiophene This suggests that it contains a ring. EXAMPLES
[0182] <Synthesis Example 2> In this example, a complex compound represented by structural formula (101) in Embodiment 1, which is one embodiment of the present invention, Ring compound, 4-[3'-(4-dibenzothienyl)-1,1'-biphenyl-4-yl] -2,6-diphenylpyrimidine (abbreviation: 2,6Ph-4pmDBTBPPm-II) The synthesis method is explained below. The structure is shown below.
[0183] [ka]
[0184] Step 1: Synthesis of 4-(4-bromophenyl)-2,6-diphenylpyrimidine The synthesis scheme of 4-(4-bromophenyl)-2,6-diphenylpyrimidine is shown below (C- 1).
[0185] [ka]
[0186] In a 300 mL three-neck flask, add 11 mL (94.6 mmol) of acetophenone and 4-bromo 17.9 g (96.7 mmol) of benzaldehyde was added and the atmosphere was replaced with nitrogen. Add 50 mL of ethanol and add 5.99 g (110.9 mmol) of sodium methoxide. A suspension in 50 mL of ethanol was added dropwise, and the mixture was stirred at room temperature for 5 hours and at 70°C for 50 minutes. After the specified time had elapsed, 15.1 g (96.6 mmol) of benzamidine hydrochloride was added to the mixture. 8.03 g (200 mmol) of sodium hydroxide was added and the mixture was stirred at 70°C for 9 hours. After a certain period of time had elapsed, the mixture was filtered under suction, and the residue was dissolved in chloroform and extracted with water. The resulting organic layer was washed with saturated saline and dried over magnesium sulfate. The mixture was gravity filtered, and the solvent was distilled off to obtain a solid. The obtained solid was washed with ethanol. After purification, the desired white solid was obtained in 8.61 g (22% yield).
[0187] In addition, the filtrate after suction filtration was concentrated and purified by silica gel column chromatography. The developing solvent was toluene. The obtained fraction was concentrated and extracted with ethanol. The resulting solid was ultrasonically washed with ethanol to obtain the desired white solid. g (yield 2.7%).
[0188] <Step 2: Synthesis of 2,6Ph-4pmDBTBPPm-II (abbreviation)> The synthesis scheme of 2,6Ph-4pmDBTBPPm-II (abbreviation) is shown in (C-2). .
[0189] [ka]
[0190] Add 5.03 g (13.0 mmol) of 4-(4-bromophenyl) 5.10 g (16.8 mmol) of 3-(diphenyl)-2,6-diphenylpyrimidine (benzothiophen-4-yl)phenylboronic acid and 0.15 g (0.49 mmol) of trimethylphenylboronic acid. bis(2-methylphenyl)phosphine, 50 mL of toluene, 16 mL of ethanol, 16 mL of 2 M potassium carbonate aqueous solution was added. The mixture was stirred under reduced pressure. The mixture was degassed, and 64 mg (0.29 mmol) of palladium acetate was added thereto. The mixture was stirred at 90° C. for 3 hours under a nitrogen stream. After the predetermined time had elapsed, the mixture was filtered under suction. Water was added to the filtrate, and the aqueous layer was extracted with toluene. The mixture was washed with water and saturated saline, and dried over magnesium sulfate. The filtrate was concentrated and combined with the residue collected after suction filtration, and dissolved in hot toluene. The mixture was filtered through Celite, alumina, and Florisil under suction. After ultrasonic cleaning with ethanol, the mixture was recrystallized with toluene to obtain the desired white solid. The amount obtained was 4.66 g (63% yield).
[0191] The resulting white solid (3.83 g) was purified by train sublimation. The white solid was heated at 280°C under conditions of 2.7 Pa and argon flow rate of 5 mL / min. After purification by sublimation, 3.39 g of a white solid was obtained, with a recovery rate of 88.6%.
[0192] The nuclear magnetic resonance spectroscopy of the compound obtained by the above synthesis method ( 1 The results of the analysis using H-NMR are shown below. As shown below.1 The H-NMR chart is shown in FIG. 11. From the results, it is clear that the above-mentioned structural formula ( 101), which is a heterocyclic compound according to one embodiment of the present invention. It was found that Pm-II (abbreviation) was obtained.
[0193] 1 H NMR(CDCl3,500MHz):δ=7.49-7.68(m, 10H) , 7.78(dd, J=7.5Hz, 2.0Hz, 2H), 7.86-7.88(m, 1 H), 7.91(d, J=8.5Hz, 2H), 8.09(s, 1H), 8.11(t, J=1.7Hz, 1H), 8.22(m, 2H), 8.32(dd, J=8.0Hz, 2 .0Hz, 2H), 8.43(d, J=8.5Hz, 2H), 8.76(dd, J=8. 0Hz, 2.0Hz, 2H).
[0194] Next, the 2,6Ph-4pmDBTBPPm-II (abbreviation) obtained in this example was Liquid Chromatography Mass Spectrometry The results were analyzed by liquid crystal / mass spectrometry (LC / MS analysis).
[0195] LC / MS analysis was performed using Waters Acquity UPLC and Waters The analysis was performed using a Xevo G2 Tof MS manufactured by Epson.
[0196] In the MS analysis, electrospray ionization was used. The capillary voltage was set at 3 The voltage was 0.0 kV, the sample cone voltage was 30 V, and detection was performed in positive mode. The components ionized under the above conditions are collided with argon gas in a collision cell. The energy of the collision of argon (collision) was The electron energy was set to 70 eV. The mass range of the measurement was m / z = 100 to 1200. It was decided.
[0197] The measurement results are shown in FIG. 12. From the results in FIG. 12, one of the compounds of the present invention represented by the structural formula (101) is The heterocyclic compound 2,6Ph-4pmDBTBPPm-II (abbreviation) is mainly Around m / z=361, around m / z=345, around m / z=258, around m / z=128 , and product ions were detected around m / z = 104. The results shown in 12 show that the characteristic Since the results show that 2,6Ph-4pmDBTBPP contained in the mixture This is important data for identifying m-II (abbreviation).
[0198] In addition, the CC bond next to the N atom of the pyrimidine ring breaks and the fragment containing the N atom Because the charge remains, the areas around m / z=361, m / z=128, and m / z=104 are In each case, the C—C bond next to the N atom of the pyrimidine ring of the compound of structural formula (100) is broken. It is useful because it is assumed that information on the At m / z=258, there are two benzothiophene rings and two benzene rings. It can be assumed that each of these product ions contains one benzene ring, which is one aspect of the present invention. The heterocyclic compound, 2,6Ph-4pmDBTBPPm-II (abbreviation), is This suggests that it contains a cyclic ring. EXAMPLES
[0199] In this example, a heterocyclic compound, 4-[3'-(4-dibenzothienyl) 2,6-diphenylpyrimidine (abbreviation: 2 ,6Ph-4mDBTBPPm-II) (structural formula (100)) was used as a part of the light-emitting layer and as an electron The light-emitting device 1 and 4-[3'-(4-dibenzothienyl)-1,1'- Biphenyl-4-yl]-2,6-diphenylpyrimidine (abbreviation: 2,6Ph-4pmD BTBPPm-II) (structural formula (101)) was used in part of the light-emitting layer and in the electron-transporting layer. The optical element 2 will be described with reference to FIG. 13. The chemical formulas of the materials used in this embodiment are as follows: As shown in.
[0200] [ka]
[0201] [ka]
[0202] <Fabrication of Light-Emitting Device 1 and Light-Emitting Device 2> First, indium tin oxide containing silicon oxide (ITSO) is deposited on a glass substrate 1100. A film was formed by sputtering to form a first electrode 1101 that functions as an anode. The film thickness was 110 nm, and the electrode area was 2 mm x 2 mm.
[0203] Next, as a pretreatment for forming a light emitting element on the substrate 1100, the substrate surface is washed with water. After baking at 200°C for 1 hour, UV ozone treatment was performed for 370 seconds.
[0204] Then, 10 -4 The substrate 1100 is introduced into a vacuum deposition apparatus whose inside has been reduced in pressure to about Pa. After vacuum baking at 170° C. for 30 minutes in a heating chamber of a vacuum deposition apparatus, the substrate 1 The 100 was allowed to cool for about 30 minutes.
[0205] Next, the substrate 1100 is vacuum-steamed so that the surface on which the first electrode 1101 is formed faces downward. In this embodiment, the EL layer 1 was formed by vacuum deposition. 102 comprises a hole injection layer 1111, a hole transport layer 1112, a light emitting layer 1113, and an electron transport A case where the layer 1114 and the electron injection layer 1115 are formed in this order will be described.
[0206] 10 minutes in the vacuum chamber -4 After depressurizing to 100 Pa, 1,3,5-tri(dibenzothiophene-4 -yl)benzene (abbreviation: DBT3P-II) and molybdenum(VI) oxide were P-II (abbreviation): molybdenum oxide = 4:2 (mass ratio) Thus, a hole injection layer 1111 was formed on the first electrode 1101. The thickness of the layer was set to 40 nm. Co-evaporation is a method of vapor deposition in which different substances are vaporized simultaneously from different sources. It is.
[0207] Next, 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine BPAFLP and 3,3'-bis(9-phenyl-9H-carbazole) The ratio of BPAFLP (abbreviation):PCCP (abbreviation) is 1:1 (mass ratio). The hole transport layer 1112 was formed by co-evaporation so as to have a thickness of 20 nm. .
[0208] Next, the light-emitting layer 1113 was formed on the hole-transporting layer 1112 .
[0209] In the case of light-emitting element 1, first, 2,6Ph-4mDBTBPPm-II (abbreviation), 4, 4'-Di(1-naphthyl)-4''-(9-phenyl-9H-carbazol-3-yl) Triphenylamine (abbreviation: PCBNBB), (acetylacetonato)bis(6-tert t-Butyl-4-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(tBu ppm)2(acac)]) to 2,6Ph-4mDBTBPPm-II (abbreviation): PC BNBB (abbreviation): [Ir(tBuppm)2(acac)] (abbreviation) = 0.5:0.5 After forming a film of 20 nm thickness by co-evaporation so that the mass ratio of the film was 0.05, a 2 ,6Ph-4mDBTBPPm-II(abbreviation):PCBNBB(abbreviation):[Ir(tBu ppm)2(acac)] (abbreviation) = 0.8:0.2:0.05 (mass ratio) The film was formed to a thickness of 20 nm, and a light emitting layer 1113 having a laminated structure and a thickness of 40 nm was formed.
[0210] In the case of light-emitting element 2, first, 2,6Ph-4pmDBTBPPm-II (abbreviation), P CBNBB (abbreviation), [Ir(tBuppm)2(acac)] (abbreviation), 2,6Ph -4pmDBTBPPm-II (abbreviation): PCBNBB (abbreviation): [Ir(tBuppm )2(acac)] (abbreviation) = 0.5:0.5:0.05 (mass ratio) After forming a 20 nm thick film using 2,6Ph-4pmDBTBPPm-II( Abbreviation): PCBNBB(Abbreviation): [Ir(tBuppm)2(acac)](Abbreviation) = 0 The thickness of the layer was 20 nm, with a mass ratio of 0.8:0.2:0.05. A light emitting layer 1113 having a thickness of 40 nm was formed.
[0211] In the light-emitting element 1 and the light-emitting element 2 described in this example, This is a structure that allows the formation of an exciplex.
[0212] Next, in the case of the light-emitting element 1, 2,6Ph-4mDBTBPPm-I was formed on the light-emitting layer 1113. I (abbreviation) was evaporated to a thickness of 10 nm, and then bathophenanthroline (abbreviation: Bphe By depositing 20 nm of SiO 2 , an electron transport layer 1114 having a laminated structure was formed. In the case of the light-emitting element 2, 2,6Ph-4pmDBTBPPm-I was formed on the light-emitting layer 1113. I (abbreviation) was evaporated to a thickness of 10 nm, and then bathophenanthroline (abbreviation: Bphe By depositing 20 nm of SiO 2 , an electron transport layer 1114 having a laminated structure was formed.
[0213] Furthermore, lithium fluoride was deposited to a thickness of 1 nm on the electron transport layer 1114 to perform electron injection. An infill layer 1115 was formed.
[0214] Finally, aluminum was evaporated onto the electron injection layer 1115 to a thickness of 200 nm. Then, a second electrode 1103 serving as a cathode was formed, and the light-emitting element 1 and the light-emitting element 2 were obtained. In the deposition process described above, the deposition was all carried out using a resistance heating method.
[0215] Table 1 shows the element structures of the thus obtained Light-emitting Element 1 and Light-emitting Element 2.
[0216] [Table 1]
[0217] The fabricated light-emitting elements 1 and 2 were placed in a nitrogen atmosphere to avoid exposure to the air. The device was sealed in a glove box (sealing material was applied around the device and the temperature was kept at 80°C during sealing). Heat treatment for 1 hour.
[0218] <Operation characteristics of light-emitting element 1 and light-emitting element 2> The operating characteristics of the fabricated light-emitting element 1 and light-emitting element 2 were measured. (Atmosphere maintained at 25°C).
[0219] First, the current density-luminance characteristics of the light-emitting element 1 and the light-emitting element 2 are shown in FIG. 14, and the voltage-luminance characteristics are shown in FIG. FIG. 15 shows the luminance-current efficiency characteristics, FIG. 16 shows the voltage-current characteristics, and FIG. 17 shows the voltage-current characteristics.
[0220] FIG. 16 shows that the light-emitting element using the heterocyclic compound of one embodiment of the present invention in the light-emitting layer and the electron-transport layer It was found that the element 1 and the light-emitting element 2 were elements with low power consumption and high efficiency.
[0221] Also, 1000cd / m 2 Main initial characteristic values of light-emitting element 1 and light-emitting element 2 in the vicinity are shown in Table 2 below.
[0222] [Table 2]
[0223] From the results of Table 2, it can be seen that the light-emitting elements 1 and 2 fabricated in this example have high luminance. It is clear that the current efficiency is high.
[0224] In addition, reliability tests were performed on the light-emitting elements 1 and 2. Results of the reliability tests This is shown in FIG. 18. In FIG. 18, the vertical axis represents the normalized brightness (%) when the initial brightness is 100%. The horizontal axis indicates the driving time (h) of the element. 0 cd / m 2 The light-emitting elements 1 and 2 were driven under a constant current density condition. As a result, the luminance of the light-emitting element 1 and the light-emitting element 2 after 100 hours was approximately 8 times lower than the initial luminance. It remained at 3%.
[0225] Therefore, the results of the reliability test show that the light-emitting element 1 and the light-emitting element 2 exhibit high reliability. In addition, by using the heterocyclic compound according to one embodiment of the present invention for a light-emitting element, It was found that a light emitting element having a long life could be obtained. EXAMPLES
[0226] <Synthesis Example 3> In this example, a heterocyclic ring represented by structural formula (112) of the first embodiment of the present invention is The compound, 4-[3'-(dibenzothiophen-4-yl)-1,1'-biphenyl-3- Synthesis of 6-phenylpyrimidine (abbreviation: 6Ph-4mDBTBPPm-II) The structure of 6Ph-4mDBTBPPm-II (abbreviation) is shown below. show.
[0227] [ka]
[0228] Step 1: Synthesis of 4-chloro-6-phenylpyrimidine 4,6-Dichloropyrimidine 5.1g, Phenylboronic acid 8.2g, Sodium carbonate 7g 0.16g, 20 mL of acetonitrile, and 20 mL of water were placed in a 100 mL round-bottom flask equipped with a reflux condenser. The mixture was then poured into a flask and the atmosphere in the container replaced with nitrogen. Add 0.347 g of dium(II) dichloride and use a microwave (2.45 GHz, 100 W) ) was irradiated for 1 hour. In addition, 2.07 g of phenylboronic acid and 1.79 g of sodium carbonate were added. The mixture was irradiated with microwaves (2.45 GHz, 100 W) for 1 hour. The organic layer was extracted with dichloromethane. The obtained organic layer was washed with water and saturated saline. The mixture was subjected to gravity filtration. The solvent in the filtrate was distilled off. The resulting residue was purified by silica column chromatography using dichloromethane as a developing solvent. The target product was obtained by purifying it with microwave irradiation (white powder, 37%). The irradiation was performed using a microwave synthesis device (CEM Discover). The synthesis scheme of the above is shown in (D-1) below.
[0229] [ka]
[0230] <Step 2: 4-[3'-(dibenzothiophen-4-yl)-1,1'-biphenyl -3-yl]-6-phenylpyrimidine (abbreviation: [6Ph-4mDBTBPPm-II] Synthesis of Next, 1.0 g of 4-chloro-6-phenylpyrimidine obtained in step 1 above, 3'-( Dibenzothiophene-4-yl)-3-biphenylboronic acid 2.0g, 2M potassium carbonate 5.3 mL of aqueous solution, 24 mL of toluene, and 3.0 mL of ethanol were added to a 100 The contents were placed in a 100 mL three-neck flask, degassed by stirring under reduced pressure, and the atmosphere inside the flask was replaced with nitrogen. To this mixture, tetrakis(triphenylphosphine)palladium(0) (abbreviation: Pd( PPh3)4) (61 mg) was added and the mixture was heated at 80°C for 7 hours to react. The organic layer was extracted with toluene, and the obtained organic layer was washed with water and saturated saline, and then dissolved in sulfuric anhydride. Magnesium was added and the mixture was gravity filtered. The solvent was removed from the solution, and the resulting residue was subjected to heat chromatography. Dissolve it in toluene and layer it in the following order: Celite, alumina, Celite, Florisil, Celite. The mixture was filtered through a filter aid, and the solvent was removed by distillation. The resulting solid was recrystallized from toluene. The synthesis scheme for step 2 is shown below. This is shown in formula (D-2).
[0231] [ka]
[0232] The obtained solid (2.4 g) was purified by train sublimation. The conditions were as follows: pressure 3.0 Pa, argon gas flow rate 15 mL / min, heating temperature 265°C. After purification by sublimation, 1.9 g of the target colorless transparent crystal was obtained with a recovery rate of 79%.
[0233] The white solid obtained in step 2 was analyzed by nuclear magnetic resonance spectroscopy ( 1 H-NMR The analysis results are shown below. 1 The H-NMR chart is shown in FIG. 6Ph-4mDBT is a heterocyclic compound according to one embodiment of the present invention, represented by structural formula (112): It was found that BPPm-II (abbreviation) was obtained.
[0234] 1 H-NMR.δ(CDCl3):7.45-7.50(dm,2H),7.52-7 .54(m,3H),7.56-7.61(m,2H),7.63-7.67(m,2H ),7.76-7.77(ds,1H),7.78(ds,1H),7.82-7.83 (dd,1H),7.85-7.87(dd,1H),8.08-8.09(ts,1H ),8.14-8.22(dm,6H),8.45-8.46(ts,1H),9.34 -9.35(ds,1H).
[0235] In addition, 6Ph-4mDBTBPPm-II (abbreviation) was analyzed by liquid chromatography mass spectrometry (LCMS). iquid chromatography mass spectrometry The analysis was performed using LC / MS (LC / MS analysis).
[0236] LC / MS analysis was performed using Waters Acquity UPLC and Waters The analysis was performed using a Xevo G2 Tof MS manufactured by Epson.
[0237] In the MS analysis, electrospray ionization was used. The capillary voltage was set at 3 The voltage was 0.0 kV, the sample cone voltage was 30 V, and detection was performed in positive mode. The components ionized under the above conditions are collided with argon gas in a collision cell. The energy of the collision of argon (collision) was The electron energies were 50 eV and 70 eV. The mass range of the measurement was m / z = 10 The range is 0 to 1200.
[0238] The measurement results are shown in Figures 20 and 21. Figure 20 shows the results when the collision energy was 50 eV. 2 and 21 are graphs showing the results when the collision energy was 70 eV. 21, the heterocyclization reaction represented by structural formula (112) according to one embodiment of the present invention is The compound 6Ph-4mDBTBPPm-II (abbreviation) is mainly around m / z=447, m Around m / z=361, around m / z=345, around m / z=258, around m / z=128, and It was found that product ions were detected around m / z = 104. The results shown in FIG. 21 show that the characteristics of 6Ph-4mDBTBPPm-II (abbreviation) Since this shows a quantitative result, it is possible to confirm that 6Ph-4mDBTBPPm- This is important data for identifying II (abbreviation).
[0239] In addition, the CC bond next to the N atom of the pyrimidine ring breaks and the fragment containing the N atom Because the charge remains, the areas around m / z=361, m / z=128, and m / z=104 are In each case, the C—C bond next to the N atom of the pyrimidine ring of the compound of structural formula (112) is broken. It is useful because it is assumed that information on the At m / z=258, there are two benzothiophene rings and two benzene rings. It can be assumed that each of these product ions contains one benzene ring, which is one aspect of the present invention. The heterocyclic compound, 6Ph-4mDBTBPPm-II (abbreviation), has a dibenzothiophene ring. This suggests that it contains EXAMPLES
[0240] <Synthesis Example 4> In this example, the 4-[ 3'-(dibenzothiophene-4-yl)-1,1'-biphenyl-3-yl]-6-( 9,9-Dimethylfluoren-2-yl)pyrimidine (abbreviation: 6FL-4mDBTBPP The synthesis method of 6FL-4mDBTBPPm (abbreviation) is as follows: As shown below.
[0241] [ka]
[0242] Step 1: 4-chloro-6-[3-(3'-dibenzothiophen-4-yl)biphenyl] Synthesis of Nylpyrimidine≫ First, 0.20 g (1.3 mmol) of 4,6-dichloropyrimidine, 3'-(dibenzo Thiophen-4-yl)-3-biphenylboronic acid 0.51 g (1.3 mmol), carbonic acid Cesium 0.85g (2.6mmol), tricyclohexylphosphine (Cy3P) 0 .2mL (0.83mmol), Tris(dibenzylideneacetone)dipalladium(0) (Pd2(dba)3) 18 mg (0.020 mmol), dioxane 10 mL, 100 The mixture was placed in a 10 mL round-bottom flask, argon bubbled for 15 minutes, and then heated in a microwave oven (85°C, The mixture was irradiated with a 150W power source for 2 hours. The aqueous layer of the resulting solution was extracted with dichloromethane. The extracted solution and the organic layer were combined and washed with water and saturated saline, and the organic layer was added with anhydrous magnesium sulfate. The mixture was gravity filtered, and the filtrate was concentrated to obtain a solid. The residue was purified by flash column chromatography using dichloromethane as a developing solvent. The mixture was then purified again by silica gel column chromatography using toluene as a developing solvent. The obtained fraction was concentrated, and the solid was recrystallized from toluene to give 4 -Chloro-6-[3-(3'-dibenzothiophen-4-yl)biphenyl]pyrimidine (white solid, 44% yield). The synthesis scheme of step 1 is shown in (E-1) below.
[0243] [ka]
[0244] <Step 2: 4-[3'-(dibenzothiophen-4-yl)(1,1'-biphenyl) -3-yl)]-6-(9,9-dimethylfluoren-2-yl)pyrimidine (abbreviation: 6 Synthesis of FL-4mDBTBPPm)≫ Next, 4-chloro-6-[3-(3'-dibenzothiophen-4-yl)biphenyl] Pyrimidine 1.0g (2.6mmol), 9,9-dimethylfluorene-2-pinacol Boronic acid 1.0 g (3.2 mmol), toluene 15 mL, ethanol 3 mL, 2 M carbonate 2.6 mL of the potassium aqueous solution was placed in a 200 mL reaction vessel, and the atmosphere in the vessel was replaced with nitrogen. Compound: Tetrakis(triphenylphosphine)palladium(0) (Pd(PPh3)4) The mixture was heated and stirred at 80° C. for 8 hours. The aqueous layer was extracted with toluene, and the resulting extract and the organic layer were combined and washed with water and saturated saline. The organic layer was dried by adding anhydrous magnesium sulfate, and the resulting mixture was subjected to gravity filtration. The filtrate was concentrated to obtain a solid, which was then purified by silica gel column chromatography. The developing solvent was toluene. The obtained fraction was concentrated to obtain a solid. This solid was recrystallized from ethanol to obtain 6FL-4mDBTBPPm (white solid The synthesis scheme of step 2 is shown below in (E-2).
[0245] [ka]
[0246] The obtained solid (0.81 g) was purified by train sublimation. The conditions were a pressure of 2.6 Pa, an argon gas flow rate of 10 mL / min, and a heating temperature of 270°C. After purification by sublimation, the target product was obtained as pale yellow transparent crystals at a recovery rate of 0.47 g (58%).
[0247] The white solid obtained in step 2 was analyzed by nuclear magnetic resonance spectroscopy ( 1 H-NMR The analysis results are shown below. 1 The H-NMR chart is shown in Figure 22. In Synthesis Example 4, the heterocyclic compound according to one embodiment of the present invention represented by the above structural formula (121) is It was found that 6FL-4mDBTBPPm (abbreviation) was obtained.
[0248] 1 H-NMR.δ(CDCl3):1.58(s,6H),7.36-7.39(m, 2H),7.43-7.50(m,3H),7.57-7.61(m,2H),7.77 -7.80(m,m),7.85(dd,2H),7.88(d,1H),8.11(t ,1H),8.14(dd,1H),8.17-8.23(m,4H),8.29(d, 1H), 8.49(t,1H), 9.37(d,1H).
[0249] In addition, 6FL-4mDBTBPPm (abbreviation) was analyzed by liquid chromatography mass spectrometry (LCMS). id Chromatography Mass Spectrometry, abbreviation: L The results were analyzed by C / MS.
[0250] LC / MS analysis was performed using Waters Acquity UPLC and Waters The analysis was performed using a Xevo G2 Tof MS manufactured by Epson.
[0251] In the MS analysis, electrospray ionization was used. The capillary voltage was set at 3 The voltage was 0.0 kV, the sample cone voltage was 30 V, and detection was performed in positive mode. The components ionized under the above conditions are collided with argon gas in a collision cell. The energy of the collision of argon (collision) was The ion energy was set to 70 eV. The mass range of the measurement was m / z = 100 to 120. The value was set to 0.
[0252] The measurement results are shown in FIG. 23. From the results in FIG. 23, one of the compounds of the present invention represented by the structural formula (121) is The heterocyclic compound 6FL-4mDBTBPPm (abbreviation) is mainly composed of m / z=5 Around 91, around m / z=547, around m / z=362, around m / z=345, m / z=2 It was found that product ions were detected around 03. The results shown in Figure 23 are as follows: Because it shows characteristic results derived from 6FL-4mDBTBPPm (abbreviation) This is important data for identifying 6FL-4mDBTBPPm (abbreviation) contained in the mixture. It can be said that this is
[0253] In addition, the CC bond next to the N atom of the pyrimidine ring breaks and the fragment containing the N atom Since the charge remains, the vicinity of m / z=362 corresponds to the N of the pyrimidine ring of the compound of structural formula (121). This is useful because it is assumed that information on the state of the CC bond next to the atom is obtained. In addition, around m / z=345, a product containing a dibenzothiophene ring and two benzene rings appears. The heterocyclic compound 6FL-4mDBTBPP, which is one embodiment of the present invention, can be assumed to be a cation. This suggests that m (abbreviation) contains a dibenzothiophene ring. EXAMPLES
[0254] In this example, a heterocyclic compound, 4-[3'-(dibenzothiophene), which is one embodiment of the present invention, is 1,1'-biphenyl-3-yl]-6-phenylpyrimidine (abbreviation: 6Ph-4mDBTBPPm-II) (structural formula (112)) was used as a part of the light-emitting layer and as an electron transport layer. The light-emitting device 3 and 4-[3'-(dibenzothiophene-4-yl)-1, 1'-biphenyl-3-yl]-6-(9,9-dimethylfluoren-2-yl)pyrimidin The emissive layer was formed of 6FL-4mDBTBPPm (structural formula (121)) The light-emitting element 4 used in the electron transport layer will be described in the same manner as in Example 3 with reference to FIG. The chemical formulas of the materials used in this example are shown below.
[0255] [ka]
[0256] <Fabrication of Light-Emitting Device 3 and Light-Emitting Device 4> First, indium tin oxide containing silicon oxide (ITSO) is deposited on a glass substrate 1100. A film was formed by sputtering to form a first electrode 1101 that functions as an anode. The film thickness was 110 nm, and the electrode area was 2 mm x 2 mm.
[0257] Next, as a pretreatment for forming a light emitting element on the substrate 1100, the substrate surface is washed with water. After baking at 200°C for 1 hour, UV ozone treatment was performed for 370 seconds.
[0258] Then, 10 -4 The substrate 1100 is introduced into a vacuum deposition apparatus whose inside has been reduced in pressure to about Pa. After vacuum baking at 170° C. for 30 minutes in a heating chamber of a vacuum deposition apparatus, the substrate 1 The 100 was allowed to cool for about 30 minutes.
[0259] Next, the substrate 1100 is vacuum-steamed so that the surface on which the first electrode 1101 is formed faces downward. In this embodiment, the EL layer 1 was formed by vacuum deposition. 102 comprises a hole injection layer 1111, a hole transport layer 1112, a light emitting layer 1113, and an electron transport A case where the layer 1114 and the electron injection layer 1115 are formed in this order will be described.
[0260] 10 minutes in the vacuum chamber -4 After depressurizing to 100 Pa, 1,3,5-tri(dibenzothiophene-4 -yl)benzene (abbreviation: DBT3P-II) and molybdenum(VI) oxide were P-II (abbreviation): molybdenum oxide = 4:2 (mass ratio) Thus, a hole injection layer 1111 was formed on the first electrode 1101. The thickness of the layer was set to 20 nm. Co-evaporation is a method of vapor deposition in which different substances are vaporized simultaneously from different sources. It is.
[0261] Next, 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine A hole transport layer 1112 was formed by evaporating BPAFLP. was set to 20 nm.
[0262] Next, the light-emitting layer 1113 was formed on the hole-transporting layer 1112 .
[0263] In the case of light-emitting element 3, first, 6Ph-4mDBTBPPm-II (abbreviation), N-(1 ,1'-biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazole-3 -yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine (abbreviation: PCB BiF), (acetylacetonato)bis(6-tert-butyl-4-phenylpyrimidinyl) Nat(III) (abbreviation: [Ir(tBuppm)2(acac)]) Ph-4mDBTBPPm-II (abbreviation): PCBBiF (abbreviation): [Ir(tBupp m)2(acac)] (abbreviation) = 0.7:0.3:0.05 (mass ratio) After forming a 20 nm thick film by deposition, 6Ph-4mDBTBPPm-II (abbreviation ):PCBBiF(abbreviation):[Ir(tBuppm)2(acac)](abbreviation)=0.8 : 0.2: 0.05 (mass ratio) with a film thickness of 20 nm and a laminated structure A light emitting layer 1113 having a thickness of 40 nm was formed.
[0264] In the case of light-emitting element 4, first 6FL-4mDBtBPPm (abbreviation), PCBBiF ( abbreviation), [Ir(tBuppm)2(acac)] (abbreviation), 6FL-4mDBTBP Pm(abbreviation): PCBBiF(abbreviation): [Ir(tBuppm)2(acac)](abbreviation The thickness of the film was 20 nm by co-evaporation so that the mass ratio of the After this, 6FL-4mDBTBPPm (abbreviation): PCBBiF (abbreviation): [Ir (tBuppm)2(acac)] (abbreviation) = 0.8:0.2:0.05 (mass ratio) Then, a 40 nm thick light emitting layer 1113 having a laminated structure is formed. Ta.
[0265] In the light-emitting element 3 and the light-emitting element 4 described in this example, This is a structure that allows the formation of an exciplex.
[0266] Next, in the case of the light-emitting element 3, 6Ph-4mDBTBPPm-II( After evaporating bathophenanthroline (abbreviation: Bphen) to a thickness of 15 nm, An electron transport layer 1114 having a laminated structure was formed by depositing 15 nm of In the case of the light-emitting element 4, 6FL-4mDBTBPPm (abbreviation) was evaporated on the light-emitting layer 1113. After the film thickness was adjusted to 15 nm, bathophenanthroline (abbreviation: Bphen) was evaporated to 10 nm. By this deposition, an electron transport layer 1114 having a laminated structure was formed.
[0267] Furthermore, lithium fluoride was deposited to a thickness of 1 nm on the electron transport layer 1114 to perform electron injection. An infill layer 1115 was formed.
[0268] Finally, aluminum was evaporated onto the electron injection layer 1115 to a thickness of 200 nm. Then, a second electrode 1103 serving as a cathode was formed, and light-emitting elements 3 and 4 were obtained. In the deposition process described above, the deposition was all carried out using a resistance heating method.
[0269] Table 3 shows the element structures of the thus obtained Light-emitting Elements 3 and 4.
[0270] [Table 3]
[0271] The fabricated light-emitting elements 3 and 4 were placed in a nitrogen atmosphere to prevent exposure to the air. The device was sealed in a glove box (sealing material was applied around the device and the temperature was kept at 80°C during sealing). Heat treatment for 1 hour.
[0272] <Operation characteristics of light-emitting element 3 and light-emitting element 4> The operating characteristics of the fabricated light-emitting element 3 and light-emitting element 4 were measured. (Atmosphere maintained at 25°C).
[0273] First, the current density-luminance characteristics of the light-emitting element 3 and the light-emitting element 4 are shown in FIG. 24 and the voltage-luminance characteristics are shown in FIG. FIG. 25 shows the luminance-current efficiency characteristics, and FIG. 26 shows the voltage-current characteristics.
[0274] FIG. 26 shows that the light-emitting element using the heterocyclic compound of one embodiment of the present invention in the light-emitting layer and the electron-transport layer It was found that the element 3 and the light-emitting element 4 were elements with low power consumption and high efficiency.
[0275] Also, 1000cd / m 2 Main initial characteristic values of light-emitting element 3 and light-emitting element 4 in the vicinity are shown in Table 4 below.
[0276] [Table 4]
[0277] From the results of Table 4, it can be seen that the light-emitting elements 3 and 4 fabricated in this example have high luminance. It is clear that the current efficiency is high.
[0278] In addition, a reliability test was performed on the light-emitting element 4. The results of the reliability test are shown in FIG. In FIG. 28, the vertical axis indicates normalized luminance (%) when the initial luminance is 100%, and the horizontal axis indicates The operating time of the element (h) is shown. The reliability test was performed with an initial luminance of 5000 cd / m 2 Set up The light-emitting element 4 was driven under a constant current density condition. After a short time, the brightness remained at approximately 83% of the initial brightness.
[0279] Therefore, the results of the reliability test show that the light-emitting element 4 exhibits high reliability. In addition, by using the heterocyclic compound according to one embodiment of the present invention in a light-emitting element, a long-life light-emitting element can be obtained. It was found that an optical element could be obtained. [Explanation of symbols]
[0280] 10 Excitplexes 11 Luminescent materials that convert triplet excitation energy into luminescence 101 Anode 102 Cathode 103 EL layer 104 Light-emitting layer 105 The first organic compound 106 Second organic compound 107 Luminous materials 201 First electrode (anode) 202 Second electrode (cathode) 203 EL layer 204 Hole injection layer 205 Hole transport layer 206 Light-emitting layer 207 Electron transport layer 208 Electron injection layer 209 The first organic compound 210 Second organic compound 211 Luminous substances 301 First electrode 302(1) First EL layer 302(2) Second EL layer 302(n-1) EL layer (n-1) 302(n) nth EL layer 304 Second electrode 305 Charge generation layer 305(1) First charge generating layer 305(2) Second charge generating layer 305(n-2) (n-2)th charge generating layer 305(n-1) (n-1)th charge generating layer 501 Element substrate 502 Pixel section 503 Driver circuit section (source line driver circuit) 504a, 504b Drive circuit section (gate line drive circuit) 505 Sealing material 506 Sealing substrate 507 Wiring 508 FPC (Flexible Printed Circuit) 509 n-channel TFT 510 p-channel TFT 511 Switching TFT 512 Current control TFT 513 First electrode (anode) 514 Insulation 515 EL layer 516 Second electrode (cathode) 517 Light emitting element 518 Space 1100 Substrate 1101 First electrode 1102 EL layer 1103 Second electrode 1111 Hole injection layer 1112 Hole transport layer 1113 Light-emitting layer 1114 Electron transport layer 1115 Electron injection layer 7100 Television equipment 7101 Case 7103 Display section 7105 Stand 7107 Display section 7109 Operation key 7110 Remote control device 7201 Main unit 7202 Case 7203 Display section 7204 Keyboard 7205 External connection port 7206 Pointing Device 7301 Case 7302 Case 7303 Connection section 7304 Display section 7305 Display section 7306 Speaker section 7307 Recording medium insertion section 7308 LED Lamp 7309 Operation key 7310 Connection terminal 7311 Sensor 7312 Microphone 7400 Mobile Phone 7401 Case 7402 Display section 7403 Operation button 7404 External connection port 7405 Speaker 7406 Mike 8001 Lighting equipment 8002 Lighting equipment 8003 Lighting equipment 8004 Lighting equipment 9033 Fastener 9034 Display mode switch 9035 Power Switch 9036 Power saving mode switch 9038 Operation switch 9630 Case 9631 Display section 9631a Display section 9631b Display section 9632a Touch Panel Area 9632b Touch Panel Area 9633 Solar Cells 9634 Charge / discharge control circuit 9635 Battery 9636 DC-DC Converter 9637 Operation key 9638 Converter 9639 Button
Claims
1. A light-emitting layer is disposed between a pair of electrodes, the light-emitting layer includes a first organic compound, a second organic compound, and a light-emitting substance that converts triplet excitation energy into light emission; the first organic compound has a pyrimidine ring and either a dibenzothiophene ring or a dibenzofuran ring; the second organic compound is an aromatic amine; The first organic compound and the second organic compound form an exciplex.
2. A light-emitting layer is disposed between a pair of electrodes, the light-emitting layer includes a first organic compound having a molecular weight of 400 or more and 1200 or less, a second organic compound, and a light-emitting substance that converts triplet excitation energy into light emission; the first organic compound has a pyrimidine ring and either a dibenzothiophene ring or a dibenzofuran ring; the second organic compound is an aromatic amine; The first organic compound and the second organic compound form an exciplex.
3. In claim 1 or 2, At least one of the pair of electrodes includes an oxide.
4. A light emitting device using the light emitting element according to claim 1 .
5. An electronic device using the light emitting device according to claim 4.
6. An illumination device using the light-emitting device according to claim 4.
Citation Information
Patent Citations
Light-emitting element, light-emitting device, display device, electronic apparatus and light device
JP2014192214A
Information processing system
JP2021179276A
Bis-carbazole derivative, material for organic electroluminescent element and organic electroluminescent element using same
WO2011132683A1
Organic electroluminescent element
WO2012176818A1
Organic electroluminescent element and display device
JP2003045662A