Secondary battery, method for manufacturing secondary battery, battery module, battery pack, and power consumption device
By using lithium tetrafluoroborate and optimizing the electrolyte composition, the crystal structure of low-cobalt or cobalt-free positive electrode active materials in secondary batteries is stabilized, improving lithium ion diffusion and overall battery performance.
Patent Information
- Application Number
- JP2024519096
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-06-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-06-24
AI Technical Summary
The challenge of stabilizing the crystal structure of low-cobalt or cobalt-free positive electrode active materials in secondary batteries to enhance lithium ion diffusion rates, thereby improving cycle life and performance, is not adequately addressed by existing technologies.
Incorporating a specific electrolyte composition containing lithium tetrafluoroborate and optimizing the content of cobalt in the positive electrode active material, along with a balanced electrolyte formulation including fluoroethylene carbonate, fluorosulfonylimide lithium salt, and fluorosulfonate lithium salt, to form stable interfacial films that enhance lithium ion diffusion and electrochemical performance.
The solution significantly improves the cycle performance, storage performance, and dynamic performance of secondary batteries by stabilizing the crystal structure and enhancing lithium ion diffusion, while maintaining high energy density and power performance.
Smart Images

Figure 2024540706000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the field of battery technology, and in particular to a secondary battery, a method for manufacturing a secondary battery, a battery module, a battery pack, and a power consuming device. [Background technology]
[0002] The secondary battery is charged and discharged by repeated absorption and desorption of lithium ions between the positive and negative electrodes, and has excellent characteristics such as high energy density, long cycle life, no pollution, and no memory effect. Therefore, as a clean energy, the secondary battery is widely used in many fields such as electronic products, energy storage power systems such as hydroelectric, thermal, wind and solar power plants, power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. Cobalt is an important component element of the positive electrode active material of the secondary battery, but the content of cobalt in the earth's crust is low, it is difficult to mine, and the price is high, so low cobalt or no cobalt is the inevitable development trend of the positive electrode active material. However, cobalt contributes greatly to the diffusion speed of lithium ions in the positive electrode active material, and low cobalt or no cobalt may reduce the diffusion speed of lithium ions in the positive electrode active material, which may affect the cycle life of the secondary battery. Summary of the Invention
[0003] The object of the present application is to provide a secondary battery, a method for manufacturing a secondary battery, a battery module, a battery pack, and a power consumption device for stabilizing the crystal structure of a low-cobalt or cobalt-free positive electrode active material and improving the diffusion rate of lithium ions therein.
[0004] According to a first aspect of the present application, there is provided a secondary battery including an electrolyte and a positive plate, the positive plate including a positive current collector and a positive film layer located on a surface of the positive current collector, the positive film layer having a molecular formula of Li a Ni b Co c M1 d M2 e O fA g [It] contains a layered material, M1 is selected from Mn, Al or a combination thereof, M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te and W, A is selected from one or more of F, N, P and S, 0.8 ≦ a ≦ 1.2, 0 < b < 0.98, 0 ≦ c < 0.1, 0 < d < 0.5, 0 ≦ e ≦ 0.5, 0 ≦ f ≦ 2, 0 ≦ g ≦ 2, b + c + d + e = 1, f + g = 2, the electrolyte contains lithium tetrafluoroborate, and based on the total mass of the electrolyte, the mass percentage of lithium tetrafluoroborate in the electrolyte is x%, and the secondary battery satisfies x > 0 and 0.05 ≦ c + x / 10 ≦ 0.15.
[0005] As a result of intensive research, the inventors of the present application have surprisingly found that by making the electrolyte contain lithium tetrafluoroborate and making the mass percentage x% of lithium tetrafluoroborate and the content c of cobalt element in the low-cobalt or cobalt-free cathode active material satisfy x > 0 and 0.05 ≦ c + x / 10 ≦ 0.15, the crystal structure of the low-cobalt or cobalt-free cathode active material can be stabilized, the diffusion rate of lithium ions inside it can be improved, and furthermore, the secondary battery can be provided with significantly improved cycle performance. In addition, the secondary battery of the present application can further have good storage performance and kinetic performance.
[0006] In any embodiment of the present application, 0.05 ≦ c + x / 10 ≦ 0.12.
[0007] In any embodiment of the present application, 0 < x ≦ 1.0.
[0008] In any embodiment of the present application, the consolidation density of the positive electrode plate is P g / cm 3 [It] is, and the secondary battery satisfies 25 ≦ P / (c + x / 10) ≦ 65, optionally 30 ≦ P / (c + x / 10) ≦ 50. Thereby, on the premise that the secondary battery has improved cycle performance and high energy density, it can have improved power performance.
[0009] In any embodiment of the present application, the consolidation density P g / cm of the positive electrode plate 3 satisfies that P is 3.3 to 3.6. This contributes to the secondary battery having a high energy density.
[0010] In any embodiment of the present application, the electrolyte further contains one or more of fluoroethylene carbonate, lithium fluorosulfonyl imide salt, and lithium fluorosulfonic acid salt. The mass percentage of fluoroethylene carbonate in the electrolyte is y1%, the mass percentage of lithium fluorosulfonyl imide salt in the electrolyte is y2%, and the mass percentage of lithium fluorosulfonic acid salt in the electrolyte is y3%. All are calculated based on the total mass of the electrolyte, and the electrolyte satisfies y1≧0, y2≧0, y3≧0, and 0<y1 + y2 + y3≦15. This contributes to forming a more stable interfacial film on the positive electrode and / or negative electrode, thereby further improving the electrochemical performance of the secondary battery.
[0011] In any embodiment of the present application, the molecular formula of the lithium fluorosulfonyl imide salt is LiN(SO2R1)(SO2R2), and R1 and R2 are each independently F or C n F 2n+1 where n is an integer from 1 to 10. Optionally, the lithium fluorosulfonyl imide salt includes lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonyl imide, or a combination thereof.
[0012] In any embodiment of the present application, the molecular formula of the lithium fluorosulfonic acid salt is LiSO3R3, and R3 represents F, a partially fluorinated or fully fluorinated C1-C10 alkyl group. Optionally, the lithium fluorosulfonic acid salt includes lithium fluorosulfonic acid, lithium trifluoromethanesulfonic acid, or a combination thereof.
[0013] In any embodiment of the present application, the mass percentage y1% of fluoroethylene carbonate in the electrolyte satisfies 0 < y1 ≤ 2.5, optionally 0 < y1 ≤ 2.0. Thereby, the interfacial film of the negative electrode can be stabilized, and the cycle performance of the secondary battery can be effectively improved.
[0014] In any embodiment of the present application, the mass percentage y1% of fluoroethylene carbonate in the electrolyte satisfies 0.5 ≤ y1 / x ≤ 4.0, optionally 0.5 ≤ y1 / x ≤ 2.0. Thereby, the synergistic effect between lithium tetrafluoroborate and fluoroethylene carbonate can be fully exerted.
[0015] In any embodiment of the present application, the mass percentage y1% of fluoroethylene carbonate in the electrolyte satisfies 0 < y1 ≤ 2.5 and 0.5 ≤ y1 / x ≤ 4.0.
[0016] In any embodiment of the present application, the mass percentage y2% of lithium fluorosulfonyl imide salt in the electrolyte satisfies 0 < y2 ≤ 14. Thereby, the rate performance and low-temperature performance of the secondary battery can be significantly improved.
[0017] In any embodiment of the present application, the mass percentage y2% of lithium fluorosulfonyl imide salt in the electrolyte satisfies 1 ≤ y2 / x ≤ 28. Thereby, the synergistic effect between lithium tetrafluoroborate and lithium fluorosulfonyl imide salt can be fully exerted.
[0018] In any embodiment of the present application, the mass percentage y2% of lithium fluorosulfonyl imide salt in the electrolyte satisfies 0 < y2 ≤ 14 and 1 ≤ y2 / x ≤ 28.
[0019] In any embodiment of the present application, when 0 < b ≤ 0.7, the mass percentage y2% of the lithium fluorosulfonylimide salt in the electrolyte satisfies 0 < y2 ≤ 5 and / or 1 ≤ y2 / x ≤ 10. Optionally, 0 < y2 ≤ 2.5, and optionally, 1 ≤ y2 / x ≤ 5.
[0020] In any embodiment of the present application, when 0.7 ≤ b < 0.98, the mass percentage y2% of the lithium fluorosulfonylimide salt in the electrolyte satisfies 5 ≤ y2 ≤ 14 and / or 10 ≤ y2 / x ≤ 28. Optionally, 8 ≤ y2 ≤ 14, and optionally, 16 ≤ y2 / x ≤ 28.
[0021] In any embodiment of the present application, the mass percentage y3% of the lithium fluorosulfonate salt in the electrolyte satisfies 0 < y3 ≤ 1.0, and optionally 0 < y3 ≤ 0.5. Thereby, the high-temperature performance of the secondary battery can be greatly improved.
[0022] In any embodiment of the present application, the mass percentage y3% of the lithium fluorosulfonate salt in the electrolyte satisfies 0.001 ≤ y3 / x ≤ 2.0, and optionally 0.001 ≤ y3 / x ≤ 1.0. Thereby, the synergistic effect between lithium tetrafluoroborate and the lithium fluorosulfonate salt can be fully exerted.
[0023] In any embodiment of the present application, the mass percentage y3% of the lithium fluorosulfonate salt in the electrolyte satisfies 0 < y3 ≤ 1.0 and 0.001 ≤ y3 / x ≤ 2.0.
[0024] In any embodiment of the present application, the electrolyte further contains fluoroethylene carbonate, a lithium fluorosulfonylimide salt and a lithium fluorosulfonate salt, and the electrolyte satisfies 0 < y1 ≤ 2.5, 0 < y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48. At this time, the overall performance of the secondary battery is further improved.
[0025] Optionally, when 0 < b ≤ 0.7, the electrolyte satisfies 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10.
[0026] Optionally, when 0.7 ≤ b < 0.98, the electrolyte satisfies 0 < y1 ≤ 2.5, 5 ≤ y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 10 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 6 ≤ y2 / y1 ≤ 48.
[0027] In any embodiment of the present application, the electrolyte satisfies the following, that is, the electrolyte further contains fluoroethylene carbonate, lithium fluorosulfonyl imide salt and lithium fluorosulfonate salt, and the electrolyte satisfies 0 < y1 ≤ 2.5, 0 < y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48, 0.036 ≤ x / (y2 + y3) ≤ 1.0. Thereby, it contributes to forming an inorganic / organic composite interface film with excellent performance on the positive electrode and the negative electrode, and thereby the overall performance of the secondary battery can be further improved.
[0028] Optionally, when 0 < b ≤ 0.7, the electrolyte satisfies 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10, 0.1 ≤ x / (y2 + y3) ≤ 1.0.
[0029] Optionally, when 0.7 ≤ b < 0.98, the electrolyte satisfies 0 < y1 ≤ 2.5, 5 ≤ y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 10 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 6 ≤ y2 / y1 ≤ 48, 0.036 ≤ x / (y2 + y3) ≤ 0.1.
[0030] In any embodiment of the present application, 0 < c < 0.1.
[0031] In any embodiment of the present application, c=0.
[0032] In any embodiment of the present application, the molecular formula is Li a Ni b Co c M1 d M2 e O f A g The weight percentage of the layered material is between 80% and 99%, optionally between 85% and 99%.
[0033] In any embodiment of the present application, the secondary battery further satisfies that the mass of the electrolyte is 10% to 20% of the total mass of the secondary battery, which is advantageous for forming a dense interface film with low impedance on the surface of the positive electrode active material.
[0034] According to a second aspect of the present application, there is provided a method for manufacturing a secondary battery, the method including a step 1 of assembling at least a positive electrode plate, a separator, a negative electrode plate, and an electrolyte into a secondary battery, the positive electrode plate including a positive electrode current collector and a positive electrode film layer located on a surface of the positive electrode current collector, the positive electrode film layer having a molecular formula of Li a Ni b Co c M1 d M2 e O f A gIt includes a layered material, where M1 is selected from Mn, Al, or a combination thereof, M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te, and W, A is selected from one or more of F, N, P, and S, 0.8 ≦ a ≦ 1.2, 0 < b < 0.98, 0 ≦ c < 0.1, 0 < d < 0.5, 0 ≦ e ≦ 0.5, 0 ≦ f ≦ 2, 0 ≦ g ≦ 2, b + c + d + e = 1, f + g = 2. The electrolyte contains lithium tetrafluoroborate, optional fluoroethylene carbonate, optional lithium fluorosulfonylimide salt, and optional lithium fluorosulfonate salt. The mass percentage of lithium tetrafluoroborate in the electrolyte is x%, the mass percentage of fluoroethylene carbonate in the electrolyte is y1%, the mass percentage of lithium fluorosulfonylimide salt in the electrolyte is y2%, and the mass percentage of lithium fluorosulfonate salt in the electrolyte is y3%, all calculated based on the total mass of the electrolyte, where x > 0, y1 ≧ 0, y2 ≧ 0, y3 ≧ 0. It includes step 1 and step 2 of selecting a secondary battery that satisfies 0.05 ≦ c + x / 10 ≦ 0.15 from the secondary battery obtained in step 1.
[0035] The secondary batteries obtained by the manufacturing method of this application can all have significantly improved cycle performance, good storage performance, and kinetic performance.
[0036] In any embodiment of this application, the method further includes the step of selecting a secondary battery that satisfies 0 < x ≦ 1.0 and 0.05 ≦ c + x / 10 ≦ 0.15 from the secondary battery obtained in step 2. At this time, the manufactured secondary battery has further improved cycle performance.
[0037] In any embodiment of this application, the method further includes the step of selecting a secondary battery that satisfies 25 ≦ P / (c + x / 10) ≦ 65 from the secondary battery obtained in step 2, where P g / cm 3represents the consolidation density of the positive electrode plate. At this time, the manufactured secondary battery can have improved power performance on the premise of significantly improved cycle performance and high energy density.
[0038] In any embodiment of the present application, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48 from the secondary battery obtained in step 2. At this time, the comprehensive performance of the manufactured secondary battery is further improved.
[0039] Optionally, when 0 < b ≤ 0.7, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10 from the secondary battery obtained in step 2.
[0040] Optionally, when 0.7 ≤ b < 0.98, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 5 ≤ y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 10 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 6 ≤ y2 / y1 ≤ 48 from the secondary battery obtained in step 2.
[0041] In any embodiment of the present application, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48, 0.036 ≤ x / (y2 + y3) ≤ 1.0 from the secondary battery obtained in step 2. At this time, the comprehensive performance of the manufactured secondary battery is further improved.
[0042] Optionally, when 0 < b ≤ 0.7, the method further includes a step of selecting a secondary battery from the secondary batteries obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10, 0.1 ≤ x / (y2 + y3) ≤ 1.0.
[0043] Optionally, when 0.7 ≤ b < 0.98, the method further includes a step of selecting a secondary battery from the secondary batteries obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 5 ≤ y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 10 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 6 ≤ y2 / y1 ≤ 48, 0.036 ≤ x / (y2 + y3) ≤ 0.1.
[0044] According to a third aspect of the present application, there is provided a battery module including the secondary battery of the first aspect of the present application or the secondary battery manufactured by the method of the second aspect of the present application.
[0045] According to a fourth aspect of the present application, there is provided a battery pack including one of the secondary battery of the first aspect of the present application, the secondary battery manufactured by the method of the second aspect of the present application, and the battery module of the third aspect of the present application.
[0046] According to a fifth aspect of the present application, there is provided an electric power consuming device including at least one of the secondary battery of the first aspect of the present application, the secondary battery manufactured by the method of the second aspect of the present application, the battery module of the third aspect of the present application, and the battery pack of the fourth aspect of the present application.
[0047] The secondary battery of the present application has significantly improved cycle performance, good storage performance, and kinetic performance. Since the battery module, battery pack, and electric power consuming device of the present application include the secondary battery according to the present application, they have at least the same advantages as the secondary battery.
Brief Description of the Drawings
[0048] In order to more clearly describe the technical solutions of the embodiments of the present application, the following briefly introduces the drawings that need to be used in the embodiments of the present application. It is obvious that the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without paying creative efforts.
[0049] [Figure 1] FIG. 1 is a schematic diagram of one embodiment of a secondary battery of the present application. [Diagram 2] FIG. 2 is an exploded schematic view of an embodiment of the secondary battery of FIG. 1. [Diagram 3] FIG. 1 is a schematic diagram of one embodiment of a battery module of the present application. [Figure 4] FIG. 1 is a schematic diagram of one embodiment of a battery pack of the present application. [Diagram 5] 5 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 4. [Figure 6] 1 is a schematic diagram of an embodiment of a power consuming device in which the secondary battery of the present application is used as a power source. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0050] Hereinafter, with appropriate reference to the drawings, embodiments specifically disclosing the secondary battery, the method for manufacturing the secondary battery, the battery module, the battery pack, and the power consumption device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of structures that are actually the same may be omitted. This is to avoid the following description becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0051] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the end values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also envisaged. It is noted that if 1 and 2 are listed as the minimum range values, and 3, 4, and 5 are listed as the maximum range values, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all envisaged. In this application, unless otherwise specified, a numerical range "a-b" represents a shorthand representation of any combination of real numbers a-b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed herein, and "0-5" is just a shorthand for combinations of these numbers. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all the embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and such technical solution should be considered to be included in the disclosure content of the present application.
[0053] Unless otherwise stated, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution, and such technical solution should be deemed to be included in the disclosure content of the present application.
[0054] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed in sequence, or steps (b) and (a) performed in sequence. For example, the method may further include step (c) as mentioned above to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0055] Unless otherwise specified, the terms "comprise" and "include" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "include" may further include or include other ingredients not listed, or may include or include only the ingredients listed.
[0056] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied when A is true (or exists) and B is false (or does not exist), when A is false (or does not exist) but B is true (or exists), and when both A and B are true (or exist).
[0057] As used in this application, the terms "plurality" and "multiple types" mean two or more than two.
[0058] A secondary battery is also called a rechargeable battery or storage battery, and refers to a battery that can continue to be used by activating the active material through a charging method after the battery is discharged. A secondary battery generally includes a positive electrode plate, a negative electrode plate, a separator, and an electrolyte. During charging and discharging of a secondary battery, lithium ions travel back and forth between the positive electrode plate and the negative electrode plate to be absorbed and desorbed. The separator is installed between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short circuits between the positive and negative electrodes, while allowing lithium ions to pass through. The electrolyte serves to conduct lithium ions between the positive electrode plate and the negative electrode plate.
[0059] During charging of the secondary battery, lithium ions are preferentially desorbed from the surface of the positive electrode active material, and then the lithium ions in the bulk phase of the positive electrode active material are timely replenished to the surface. The cobalt element in the positive electrode active material affects the ionic conductivity properties of the positive electrode active material as follows: (1) When the content of the cobalt element in the positive electrode active material is high, the lithium ions in the bulk phase can be timely replenished to the surface of the positive electrode active material; (2) When the content of the cobalt element in the positive electrode active material is low, the lithium ions in the bulk phase cannot be timely replenished to the surface of the positive electrode active material, but the lithium ions on the surface have already been desorbed, which causes excessive lithium desorption on the surface of the positive electrode active material, thereby affecting the crystal structure of the positive electrode active material (for example, the irreversible distortion of the positive electrode active material and the increase in the number of lattice defects), and reducing the cycle performance of the secondary battery.
[0060] In addition, the cobalt element can further stabilize the crystal structure of the positive electrode active material. When the content of the cobalt element in the positive electrode active material is reduced or does not contain the cobalt element, the dissolution rate of metal ions, especially manganese ions, in the positive electrode active material becomes faster. The dissolved manganese ions are reduced to metal manganese after moving to the negative electrode. These formed metal manganese correspond to a "catalyst" and can catalyze the decomposition of the SEI film (solid electrolyte interphase) on the surface of the negative electrode. Some of the by-products generated are gaseous and are prone to causing battery expansion, affecting the safety of the secondary battery, and the other part is deposited on the surface of the negative electrode, blocking the passage of lithium ions entering and exiting the negative electrode, resulting in an increase in the impedance of the secondary battery, and affecting the dynamic performance of the secondary battery. In addition, in order to compensate for the loss of the SEI film, the electrolyte and the active lithium ions inside the battery are constantly consumed, which has an irreversible effect on the capacity retention rate of the secondary battery.
[0061] Therefore, it is important and practical to stabilize the crystal structure of low-cobalt or cobalt-free positive electrode active materials and improve the diffusion rate of lithium ions therein. Researchers have been working hard to improve the diffusion rate of lithium ions in low-cobalt or cobalt-free positive electrode active materials, but no desirable solution has been found at present.
[0062] As a result of intensive research, the inventors of the present application unexpectedly discovered that, by making the electrolyte contain an appropriate amount of lithium tetrafluoroborate and by making the content of lithium tetrafluoroborate and the content of cobalt element in the positive electrode active material satisfy a specific relational formula, it is possible to stabilize the crystal structure of the low-cobalt or cobalt-free positive electrode active material and improve the diffusion rate of lithium ions therein.
[0063] secondary battery Specifically, an embodiment of the present application provides a secondary battery, which includes an electrolyte and a positive plate. The positive plate includes a positive current collector and a positive film layer located on the surface of the positive current collector, the positive film layer having a molecular formula of Lia Ni b Co c M1 d M2 e O f A g It includes a layered material which is as follows: M1 is selected from Mn, Al or a combination thereof, M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te and W, A is selected from one or more of F, N, P and S, 0.8≦a≦1.2, 0<b<0.98, 0≦c<0.1, 0<d<0.5, 0≦e≦0.5, 0≦f≦2, 0≦g≦2, b + c + d + e = 1, f + g = 2. The electrolyte contains lithium tetrafluoroborate (LiBF4). Based on the total mass of the electrolyte, the mass percentage of lithium tetrafluoroborate in the electrolyte is x%, and the secondary battery satisfies x>0 and 0.05≦c + x / 10≦0.15.
[0064] The electrolyte is one of the important factors affecting the performance of a secondary battery. Currently, the most widely commercially applied electrolyte system is a mixed carbonate solution of lithium hexafluorophosphate. However, lithium hexafluorophosphate has low thermal stability in a high-temperature environment and decomposes at high temperatures to produce PF5. PF5 has high Lewis acidity and acts on the lone pair of electrons on the oxygen atom in the organic solvent molecule to decompose the organic solvent. Moreover, PF5 also has high sensitivity to trace amounts of moisture in the electrolyte. When it comes into contact with water, HF is generated, thereby increasing the acidity of the electrolyte, further corroding the positive electrode active material and the positive electrode current collector, and easily causing the elution of transition metal ions in the positive electrode active material. As a result, lithium hexafluorophosphate cannot only improve the diffusion rate of lithium ions in the low-cobalt or cobalt-free positive electrode active material, but also corrode the positive electrode active material and easily destroy its crystal structure. Therefore, it is necessary to improve the electrolyte.
[0065] The inventors of the present application have unexpectedly found through extensive research that the electrolyte contains lithium tetrafluoroborate, and the mass percentage x% of lithium tetrafluoroborate and the content c of cobalt element in the low-cobalt or cobalt-free positive electrode active material satisfy x>0 and 0.05≦c+x / 10≦0.15, so that the crystal structure of the low-cobalt or cobalt-free positive electrode active material can be stabilized, the diffusion speed of lithium ions therein can be improved, and the secondary battery can have significantly improved cycle performance. In addition, the secondary battery of the present application can also have good storage performance and dynamic performance.
[0066] Although the mechanism is still unclear, the inventors speculate that the following may be possible causes.
[0067] First, when the mass percentage x% of lithium tetrafluoroborate and the content c of cobalt element in the low-cobalt or cobalt-free positive electrode active material satisfy x>0 and 0.05≦c+x / 10≦0.15, lithium tetrafluoroborate can form a dense and low-impedance interfacial film on the surface of the positive electrode active material, and the B atoms in lithium tetrafluoroborate can be sufficiently bonded with the O atoms in the positive electrode active material, thereby reducing the charge transfer impedance of the positive electrode active material, reducing the diffusion resistance of lithium ions in the bulk phase of the positive electrode active material, avoiding excessive lithium desorption on the surface of the positive electrode active material, and stabilizing the crystal structure of the positive electrode active material. The crystal structure of the positive electrode active material of the present application is more stable, and therefore the probability of problems such as unstable structural, chemical or electrochemical properties of the positive electrode active material due to excessive lithium desorption on the surface is further reduced. Therefore, the secondary battery of the present application can have improved electrochemical performance, and in particular, can have significantly improved cycle performance.
[0068] Secondly, when the mass percentage x% of lithium tetrafluoroborate and the content c of cobalt element in the low-cobalt or cobalt-free positive electrode active material satisfy x>0 and 0.05≦c+x / 10≦0.15, lithium tetrafluoroborate can form a dense and low-impedance interfacial film on the surface of the positive electrode active material, effectively reducing the direct contact between the positive electrode active material and the electrolyte, while reducing the surface oxygen activity of the positive electrode active material. This can reduce the oxidative decomposition of the electrolyte at the positive electrode, reduce the amount of transition metal ions leaching, and further improve the electrochemical performance of the secondary battery, such as reducing the irreversible consumption of active lithium ions, reducing the volume expansion rate of the battery, and reducing the positive electrode interface impedance. Therefore, the secondary battery of the present application can further have good storage performance and dynamic performance.
[0069] Third, lithium tetrafluoroborate has high thermal stability and low sensitivity to moisture, which can improve the high-temperature stability of the secondary battery.
[0070] When c+x / 10<0.05, the content of lithium tetrafluoroborate in the electrolyte is insufficient to form a dense and low impedance interfacial film on the surface of the low-cobalt or cobalt-free positive electrode active material, and lithium tetrafluoroborate cannot effectively reduce the charge transfer impedance of the low-cobalt or cobalt-free positive electrode active material, and cannot effectively reduce the diffusion resistance of lithium ions in the bulk phase of the low-cobalt or cobalt-free positive electrode active material to suppress excessive lithium desorption from the surface of the low-cobalt or cobalt-free positive electrode active material. Therefore, the secondary battery is difficult to have significantly improved cycle performance. When c+x / 10>0.15, the content of lithium tetrafluoroborate in the electrolyte is too high, and its solubility in the electrolyte is low, so that the electrolyte contains lithium tetrafluoroborate in a molecular state that is not completely dissociated, which is prone to precipitation in the electrolyte, especially in a low-temperature environment, and further increases safety risks such as separator penetration, so that the safety performance and cycle performance of the secondary battery are both poor, and the precipitated lithium tetrafluoroborate further destroys the interface of the electrode, thereby causing an increase in self-discharge of the secondary battery. In some embodiments, optionally, 0.05≦c+x / 10≦0.14, 0.05≦c+x / 10≦0.13, 0.05≦c+x / 10≦0.12, 0.05≦c+x / 10≦0.11, or 0.05≦c+x / 10≦0.10.
[0071] In the present application, the mass percentage x% of lithium tetrafluoroborate satisfies x>0. When the content of lithium tetrafluoroborate is high, its solubility in the electrolyte is low, so that the electrolyte contains lithium tetrafluoroborate in a molecular state that is not completely dissociated, which is prone to precipitate in the electrolyte, particularly in a low-temperature environment, and further increases safety risks such as separator penetration. Therefore, when the content of lithium tetrafluoroborate is high, the safety performance and cycle performance of the secondary battery may be deteriorated. In addition, the precipitated lithium tetrafluoroborate further destroys the interface of the electrode, thereby causing an increase in self-discharge of the secondary battery. In some embodiments, optionally, 0 <x≦1.0である。
[0072] According to further research by the inventors of this application, the content of cobalt element in the positive electrode active material further affects the electronic conductivity properties of the positive electrode active material as follows: (1) when the content of cobalt element in the positive electrode active material is high, the positive electrode active material has good electronic conductivity properties; (2) when the content of cobalt element in the positive electrode active material is low, the electronic conductivity properties of the positive electrode active material are poor, and the power performance of the secondary battery is poor. In addition, the larger the compaction density of the positive electrode plate, the worse the power performance of the secondary battery. Therefore, in order to ensure good power performance of the secondary battery, the countermeasure generally adopted in the prior art is to reduce the compaction density of the positive electrode plate, which leads to a loss of energy density of the secondary battery.
[0073] According to the unexpected discovery of the inventors of the present application, the compaction density P g / cm 3When the mass percentage of lithium tetrafluoroborate x% and the content c of cobalt element in the low-cobalt or cobalt-free positive electrode active material further satisfy 25≦P / (c+x / 10)≦65, the secondary battery can have improved power performance under the premise of improved cycle performance and high energy density, for example, the initial power and power increase during cycling of the secondary battery are both significantly improved. Although the mechanism is still unclear, the inventor speculates that the following possible causes are considered. First, when the content of lithium tetrafluoroborate is within a suitable range, the crystal structure of the low-cobalt or cobalt-free positive electrode active material can be stabilized, thereby providing good electronic conductive properties; second, the appropriate compaction density contributes to the formation of a good electronic conductive network in the positive plate.
[0074] Therefore, when 25≦P / (c+x / 10)≦65, the secondary battery can have improved power performance under the premise of improved cycle performance and high energy density. And the following situation can be effectively avoided: when P / (c+x / 10)<25, the compaction density of the positive plate may be low, which may cause the electronic conductive network in the positive plate to be poor, and the power performance of the secondary battery cannot be effectively improved, and the energy density of the secondary battery may be sacrificed; or the content of lithium tetrafluoroborate may be high, which may cause the stability of the negative electrode interfacial film to be reduced, and further cause the internal resistance of the battery to increase and the power performance to deteriorate; when P / (c+x / 10)>65, the content of lithium tetrafluoroborate may be insufficient to compensate for the deterioration of the power performance of the secondary battery caused by the increase in the compaction density of the positive plate, which may also cause the power performance of the secondary battery to deteriorate. Optionally, 25≦P / (c+x / 10)≦60, 25≦P / (c+x / 10)≦55, 25≦P / (c+x / 10)≦50, 25≦P / (c+x / 10)≦45, 25≦P / (c+x / 10)≦40, 30≦P / (c+x / 10)≦65, 30≦P / (c+x / 10)≦60, 30≦P / (c+x / 10)≦55, 30≦P / (c+x / 10)≦50, or 30≦P / (c+x / 10)≦45.
[0075] In some embodiments, optionally, the consolidation density P g / cm of the positive electrode plate 3 is such that P is 3.3 to 3.6, and further optionally 3.4 to 3.5. This contributes to the secondary battery having a high energy density.
[0076] [Electrolyte] In some embodiments, the electrolyte may further contain one or more of fluoroethylene carbonate (FEC), lithium fluorosulfonylimide salt, and lithium fluorosulfonate salt in addition to lithium tetrafluoroborate. The mass percentage of fluoroethylene carbonate in the electrolyte is y1%, the mass percentage of lithium fluorosulfonylimide salt in the electrolyte is y2%, and the mass percentage of lithium fluorosulfonate salt in the electrolyte is y3%. All are calculated based on the total mass of the electrolyte, and the electrolyte satisfies y1≧0, y2≧0, y3≧0, and 0<y1 + y2 + y3≦15. Lithium tetrafluoroborate can form a dense and low-impedance interfacial film on the surface of the positive electrode active material, but the long-term stability of the interfacial film formed on the negative electrode by lithium tetrafluoroborate is low. Therefore, when the electrolyte further contains the above compounds, it contributes to forming a more stable interfacial film on the positive electrode and / or the negative electrode, thereby further improving the electrochemical performance of the secondary battery.
[0077] In some embodiments, the electrolyte may further contain fluoroethylene carbonate. Optionally, the mass percentage y1% of fluoroethylene carbonate satisfies 0<y1≦2.5. For example, y1 may be in the range composed of 0.10, 0.20, 0.50, 0.75, 1.0, 1.25, 1.50, 1.75, 2.0, 2.5, or any numerical value above. Further optionally, 0<y1≦2.0, 0<y1≦1.75, 0<y1≦1.5, 0<y1≦1.25, 0<y1≦1.0, 0<y1≦0.75, or 0<y1≦0.5.
[0078] For secondary batteries, fluoroethylene carbonate undergoes a reductive decomposition reaction at high potential, and can form a SEI film with a certain ductility on the surface of the negative electrode active material, while suppressing the reductive decomposition of the organic solvent at low potential and suppressing the absorption of the organic solvent into the negative electrode active material. Therefore, when the electrolyte further contains fluoroethylene carbonate, it can stabilize the interface film of the negative electrode, thereby effectively improving the cycle performance of the secondary battery. In addition, fluoroethylene carbonate is resistant to high-pressure oxidation, which is favorable for matching with high-voltage positive electrode active materials, and is therefore favorable for improving the energy density of the secondary battery. However, when fluoroethylene carbonate decomposes under high temperature, it forms HF, which increases the acidity of the electrolyte, destroys the structural stability of the positive electrode active material, and increases the amount of gas generated by the secondary battery, thereby deteriorating the high-temperature storage performance of the secondary battery. Therefore, the content of fluoroethylene carbonate should not be too high.
[0079] In some embodiments, the mass percentage x% of lithium tetrafluoroborate and the mass percentage y1% of fluoroethylene carbonate may further satisfy 0.5≦y1 / x≦4.0. The inventors of the present application unexpectedly discovered that when the relationship between the mass percentage x% of lithium tetrafluoroborate and the mass percentage y1% of fluoroethylene carbonate is reasonably controlled to satisfy 0.5≦y1 / x≦4.0, the synergistic effect between lithium tetrafluoroborate and fluoroethylene carbonate can be fully exerted, which not only does not significantly increase the gas generation amount of the secondary battery, but also further improves the cycle performance of the secondary battery. The possible cause is as follows: lithium tetrafluoroborate is a stabilizer for the positive electrode active material, and the B atom in its structure has the function of interacting with the O atom on the surface of the positive electrode active material, which can suppress the destruction of the structure of the positive electrode active material by HF. Optionally, 0.5≦y1 / x≦3.5, 0.5≦y1 / x≦3.0, 0.5≦y1 / x≦2.5, 0.5≦y1 / x≦2.0, 0.5≦y1 / x≦1.5, 0.5≦y1 / x≦1.0.
[0080] In some embodiments, the electrolyte may further contain a lithium fluorosulfonyl imide salt. The molecular formula of the lithium fluorosulfonyl imide salt may be LiN(SO2R1)(SO2R2), where R1 and R2 are each independently F or C n F 2n+1 is represented, and n is an integer from 1 to 10. Optionally, the lithium fluorosulfonyl imide salt includes lithium bis(fluorosulfonyl)imide (LiFSI), lithium trifluoromethanesulfonyl imide (LiTFSI), or a combination thereof.
[0081] Optionally, the mass percentage y2% of the lithium fluorosulfonyl imide salt satisfies 0 < y2 ≤ 14. For example, y2 may be in the range composed of 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or any numerical value above.
[0082] The fluorosulfonyl imide anion is a weakly coordinating anion centered on N, with a conjugated group and highly electron-withdrawing -F or -C n F 2n+1The anion charge is highly delocalized, and the interaction between the anion and the lithium ion is weak. Therefore, the fluorosulfonylimide lithium salt has low lattice energy and is easy to dissociate, thereby increasing the ionic conductivity of the electrolyte, reducing the viscosity of the electrolyte, and improving the rate performance and low-temperature performance of the secondary battery. In addition, the fluorosulfonylimide lithium salt has the characteristics of high thermal stability and resistance to hydrolysis, thereby forming a thinner SEI film on the surface of the negative electrode active material, which has lower impedance and higher thermal stability, thereby reducing the side reaction between the negative electrode active material and the electrolyte. Therefore, when the electrolyte further contains fluorosulfonylimide lithium salt, the rate performance and low-temperature performance of the secondary battery can be significantly improved. However, the fluorosulfonylimide lithium salt cannot withstand high pressure, and may corrode the positive electrode current collector (e.g., aluminum foil) at high potential and increase the side reaction between the positive electrode active material and the electrolyte, which is likely to affect the cycle performance of the secondary battery. Therefore, the content of the fluorosulfonylimide lithium salt should not be too high.
[0083] In some embodiments, the mass percentage x% of lithium tetrafluoroborate and the mass percentage y2% of lithium fluorosulfonyl imide salt may further satisfy 1 ≦ y2 / x ≦ 28. According to the unexpected discovery of the inventors of the present application, when the relationship between the mass percentage x% of lithium tetrafluoroborate and the mass percentage y2% of lithium fluorosulfonyl imide salt is reasonably controlled to satisfy 1 ≦ y2 / x ≦ 28, the synergistic effect between lithium tetrafluoroborate and lithium fluorosulfonyl imide salt can be fully exerted, not only significantly deteriorating the cycle performance of the secondary battery, but also further improving the rate performance and low-temperature performance of the secondary battery. The following reasons may be considered as possible causes, that is, lithium tetrafluoroborate, as a stabilizer of the positive electrode active material, can form a dense and low-impedance interfacial film on the surface of the positive electrode active material, suppressing the side reaction between the positive electrode active material and the electrolyte, and lithium tetrafluoroborate has a passivation effect on the positive electrode current collector, which can be preferentially oxidized and decomposed on the surface of the positive electrode current collector to form a layer of passivation film, thereby effectively improving the corrosion of the positive electrode current collector by the lithium fluorosulfonyl imide salt.
[0084] According to further research by the inventors, the content b of nickel element in the positive electrode active material affects the improvement effect of the lithium fluorosulfonyl imide salt on the performance of the secondary battery. When the content of nickel element is high, the thermal stability of the positive electrode active material is low, and the high-temperature capacity attenuation is fast. Therefore, when a higher content of lithium fluorosulfonyl imide salt is adopted, the improvement effect on the high-temperature performance of the secondary battery is more significant. When the content of nickel element is low, the thermal stability of the positive electrode active material is high, and with the increase of the content of lithium fluorosulfonyl imide salt in the electrolyte, the improvement effect on the high-temperature performance of the secondary battery does not increase continuously.
[0085] In some embodiments, when 0 < b ≦ 0.7, the mass percentage y2% of the lithium fluorosulfonyl imide salt in the electrolyte satisfies 0 < y2 ≦ 5 and / or 1 ≦ y2 / x ≦ 10.
[0086] Optionally, 0 < y2 ≤ 4.5, 0 < y2 ≤ 4, 0 < y2 ≤ 3.5, 0 < y2 ≤ 3, 0 < y2 ≤ 2.5, 0 < y2 ≤ 2, 0 < y2 ≤ 1.5, or 0 < y2 ≤ 1.
[0087] Optionally, 1 ≤ y2 / x ≤ 9, 1 ≤ y2 / x ≤ 8, 1 ≤ y2 / x ≤ 7, 1 ≤ y2 / x ≤ 6, 1 ≤ y2 / x ≤ 5, 1 ≤ y2 / x ≤ 4, 1 ≤ y2 / x ≤ 3, or 1 ≤ y2 / x ≤ 2.
[0088] In some embodiments, when 0.7 ≤ b < 0.98, the mass percentage y2% of the lithium fluorosulfonylimide salt in the electrolyte satisfies 5 ≤ y2 ≤ 14 and / or 10 ≤ y2 / x ≤ 28.
[0089] Optionally, 5 ≤ y2 ≤ 13, 5 ≤ y2 ≤ 12, 5 ≤ y2 ≤ 11, 5 ≤ y2 ≤ 10, 6 ≤ y2 ≤ 14, 6 ≤ y2 ≤ 13, 6 ≤ y2 ≤ 12, 6 ≤ y2 ≤ 11, 6 ≤ y2 ≤ 10, 7 ≤ y2 ≤ 14, 7 ≤ y2 ≤ 13, 7 ≤ y2 ≤ 12, 7 ≤ y2 ≤ 11, 7 ≤ y2 ≤ 10, 8 ≤ y2 ≤ 14, 8 ≤ y2 ≤ 13, 8 ≤ y2 ≤ 12, 8 ≤ y2 ≤ 11, or 8 ≤ y2 ≤ 10.
[0090] Optionally, 12 ≤ y2 / x ≤ 28, 12 ≤ y2 / x ≤ 26, 12 ≤ y2 / x ≤ 24, 12 ≤ y2 / x ≤ 22, 12 ≤ y2 / x ≤ 20, 14 ≤ y2 / x ≤ 28, 14 ≤ y2 / x ≤ 26, 14 ≤ y2 / x ≤ 24, 14 ≤ y2 / x ≤ 22, 14 ≤ y2 / x ≤ 20, 16 ≤ y2 / x ≤ 28, 16 ≤ y2 / x ≤ 26, 16 ≤ y2 / x ≤ 24, 16 ≤ y2 / x ≤ 22, or 16 ≤ y2 / x ≤ 20.
[0091] In some embodiments, the electrolyte may further contain lithium fluorosulfonate salt. The molecular formula of the lithium fluorosulfonate salt may be LiSO3R3, where R3 represents F, a partially fluorinated or fully fluorinated C1-C10 alkyl group. Optionally, the lithium fluorosulfonate salt includes lithium fluorosulfonate, lithium trifluoromethanesulfonate, or a combination thereof.
[0092] Optionally, the mass percentage y3% of the lithium fluorosulfonate salt satisfies 0 < y3 ≦ 1.0. For example, y3 may be in the range composed of 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.0, or any numerical value above. Further optionally, 0 < y3 ≦ 0.9, 0 < y3 ≦ 0.8, 0 < y3 ≦ 0.7, 0 < y3 ≦ 0.6, 0 < y3 ≦ 0.5, 0 < y3 ≦ 0.4, 0 < y3 ≦ 0.3, or 0 < y3 ≦ 0.2.
[0093] The lithium fluorosulfonate salt can not only form an interfacial film on the surface of the negative electrode active material, but also form an interfacial film on the surface of the positive electrode active material. At the same time, it has high thermal stability, which greatly improves the charge and discharge characteristics of the secondary battery at high temperatures, increases the high-temperature cycle capacity retention rate of the secondary battery, and can suppress the generation of gas. However, the ionic conductivity of the lithium fluorosulfonate salt is low and it is likely to affect the kinetic performance of the secondary battery. Therefore, the content of the lithium fluorosulfonate salt should not be too high.
[0094] In some embodiments, the mass percentage x% of lithium tetrafluoroborate and the mass percentage y3% of lithium fluorosulfonate may further satisfy 0.001 ≦ y3 / x ≦ 2.0. According to the unexpected discovery of the inventor of the present application, when the relationship between the mass percentage x% of lithium tetrafluoroborate and the mass percentage y3% of lithium fluorosulfonate is reasonably controlled to satisfy 0.001 ≦ y3 / x ≦ 2.0, the synergistic effect between lithium tetrafluoroborate and lithium fluorosulfonate can be fully exerted, thereby contributing to the formation of a dense, stable and low-impedance interfacial film on the positive and negative electrodes, and further improving the high-temperature performance of the secondary battery. For example, it can improve the high-temperature cycle performance and high-temperature storage performance, and does not significantly deteriorate the kinetic performance of the secondary battery. Optionally, 0.001 ≦ y3 / x ≦ 1.5, 0.001 ≦ y3 / x ≦ 1.25, 0.001 ≦ y3 / x ≦ 1.0, 0.001 ≦ y3 / x ≦ 0.75, 0.001 ≦ y3 / x ≦ 0.5, or 0.001 ≦ y3 / x ≦ 0.25.
[0095] In some embodiments, the electrolyte may further contain any two of fluoroethylene carbonate, lithium fluorosulfonylimide salt, and lithium fluorosulfonate.
[0096] For example, in some embodiments, the electrolyte may contain a combination of fluoroethylene carbonate and lithium fluorosulfonylimide salt. Optionally, the mass percentage y1% of the fluoroethylene carbonate satisfies 0 < y1 ≦ 2.5, the mass percentage y2% of the lithium fluorosulfonylimide salt satisfies 0 < y2 ≦ 14, and 0 < y1 + y2 ≦ 15.
[0097] Optionally, the mass percentage x% of lithium tetrafluoroborate, the mass percentage y1% of fluoroethylene carbonate, and the mass percentage y2% of the fluorosulfonylimide lithium salt further satisfy 0.5≦y1 / x≦4.0 and / or 1≦y2 / x≦28, thereby providing the secondary battery with significantly improved cycle performance, as well as improved rate performance and low temperature performance.
[0098] Optionally, the mass percentage y1% of the fluoroethylene carbonate and the mass percentage y2% of the fluorosulfonylimide lithium salt may further satisfy 0.5≦y2 / y1≦48.
[0099] Further optionally, the mass percentage of lithium tetrafluoroborate is x%, the mass percentage of fluoroethylene carbonate is y1%, and the mass percentage of fluorosulfonylimide lithium salt is y2%, and simultaneously satisfy 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, and 0.5≦y2 / y1≦48. Fluoroethylene carbonate can effectively improve the cycle performance of the secondary battery, fluorosulfonylimide lithium salt can improve the rate performance and low temperature performance of the secondary battery, and lithium tetrafluoroborate, as a stabilizer for the positive electrode active material, can form a dense and low impedance interfacial film on the surface of the positive electrode active material, significantly improve the diffusion rate of lithium ions in the low-cobalt or cobalt-free positive electrode active material, and inhibit the side reaction between the positive electrode active material and the electrolyte, and inhibit the destruction of the structure of the positive electrode active material by HF. Therefore, by further rationally adjusting the content relationship among the three components to simultaneously satisfy 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, and 0.5≦y2 / y1≦48, the synergistic effect among the three components can be fully exerted, which is advantageous in fully suppressing the defects that occur when each component is used alone, and also enables the formation of a positive electrode interfacial film and a negative electrode interfacial film that are dense, stable, and have low impedance.
[0100] In particular, when 0 < b ≤ 0.7, the electrolyte may satisfy 0 < y1 ≤ 2.5 and 0 < y2 ≤ 5. Optionally, the electrolyte may further satisfy 0.5 ≤ y1 / x ≤ 4.0 and 1 ≤ y2 / x ≤ 10. Further optionally, the electrolyte may further satisfy 0.5 ≤ y2 / y1 ≤ 10.
[0101] In particular, when 0.7 ≤ b < 0.98, the electrolyte may satisfy 0 < y1 ≤ 2.5 and 5 ≤ y2 ≤ 14. Optionally, the electrolyte may further satisfy 0.5 ≤ y1 / x ≤ 4.0 and 10 ≤ y2 / x ≤ 28. Further optionally, the electrolyte may further satisfy 6 ≤ y2 / y1 ≤ 48.
[0102] For example, in some embodiments, the electrolyte may include a combination of fluoroethylene carbonate and lithium fluorosulfonate salt. Optionally, the mass percentage y1% of the fluoroethylene carbonate satisfies 0 < y1 ≤ 2.5, and the mass percentage y3% of the lithium fluorosulfonate salt satisfies 0 < y3 ≤ 1.0. Further optionally, the mass percentage x% of lithium tetrafluoroborate, the mass percentage y1% of fluoroethylene carbonate, and the mass percentage y3% of lithium fluorosulfonate salt further satisfy 0.5 ≤ y1 / x ≤ 4.0 and / or 0.001 ≤ y3 / x ≤ 2.0. Thereby, the secondary battery has significantly improved cycle performance and at the same time improved high-temperature performance.
[0103] For example, in some embodiments, the electrolyte may include a combination of lithium fluorosulfonyl imide salt and lithium fluorosulfonate salt. Optionally, the mass percentage y2% of the lithium fluorosulfonyl imide salt satisfies 0 < y2 ≤ 14, the mass percentage y3% of the lithium fluorosulfonate salt satisfies 0 < y3 ≤ 1.0, and 0 < y2 + y3 ≤ 15.
[0104] Optionally, the mass percentage x% of lithium tetrafluoroborate, the mass percentage y2% of lithium fluorosulfonylimide salt and the mass percentage y3% of lithium fluorosulfonate salt further satisfy 1 ≤ y2 / x ≤ 28 and / or 0.001 ≤ y3 / x ≤ 2.0. Thereby, the secondary battery has significantly improved cycle performance and at the same time has improved rate performance, low-temperature performance and high-temperature performance. Further optionally, the mass percentage x% of lithium tetrafluoroborate, the mass percentage y2% of lithium fluorosulfonylimide salt and the mass percentage y3% of lithium fluorosulfonate salt simultaneously satisfy 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, and 0.036 ≤ x / (y2 + y3) ≤ 1.0. This contributes to forming an inorganic / organic composite interface film with excellent performance on the positive electrode and the negative electrode, and thereby the overall performance of the secondary battery can be further improved.
[0105] In particular, when 0 < b ≤ 0.7, the electrolyte may satisfy 0 < y2 ≤ 5 and 0 < y3 ≤ 1.0. Optionally, the electrolyte may further satisfy 1 ≤ y2 / x ≤ 10 and 0.001 ≤ y3 / x ≤ 2.0. Further optionally, the electrolyte may further satisfy 0.1 ≤ x / (y2 + y3) ≤ 1.0.
[0106] In particular, when 0.7 ≤ b < 0.98, the electrolyte may satisfy 5 ≤ y2 ≤ 14 and 0 < y3 ≤ 1.0. Optionally, the electrolyte may further satisfy 10 ≤ y2 / x ≤ 28 and 0.001 ≤ y3 / x ≤ 2.0. Further optionally, the electrolyte may further satisfy 0.036 ≤ x / (y2 + y3) ≤ 0.1.
[0107] In some embodiments, the electrolyte may simultaneously contain fluoroethylene carbonate, lithium fluorosulfonyl imide salt, and lithium fluorosulfonic acid salt. Optionally, the mass percentage y1% of the fluoroethylene carbonate satisfies 0 < y1 ≤ 2.5, the mass percentage y2% of the lithium fluorosulfonyl imide salt satisfies 0 < y2 ≤ 14, the mass percentage y3% of the lithium fluorosulfonic acid salt satisfies 0 < y3 ≤ 1.0, and 0 < y1 + y2 + y3 ≤ 15.
[0108] Optionally, the electrolyte further satisfies 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, and 0.001 ≤ y3 / x ≤ 2.0. Thereby, the secondary battery has significantly improved cycle performance, and at the same time, improved rate performance, low-temperature performance, and high-temperature performance. Further optionally, the electrolyte simultaneously satisfies 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, and 0.5 ≤ y2 / y1 ≤ 48. At this time, the overall performance of the secondary battery is further improved. Further optionally, the electrolyte simultaneously satisfies 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48, and 0.036 ≤ x / (y2 + y3) ≤ 1.0. This contributes to forming an inorganic / organic composite interface film with excellent performance on the positive and negative electrodes, thereby further improving the overall performance of the secondary battery.
[0109] In particular, when 0 < b ≤ 0.7, the electrolyte may satisfy 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, and 0 < y3 ≤ 1.0. Optionally, the electrolyte may further satisfy 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, and 0.001 ≤ y3 / x ≤ 2.0. Further optionally, the electrolyte may further satisfy 0.5 ≤ y2 / y1 ≤ 10 and / or 0.1 ≤ x / (y2 + y3) ≤ 1.0.
[0110] In particular, when 0.7 ≦ b < 0.98, the electrolytic solution may satisfy 0 < y1 ≦ 2.5, 5 ≦ y2 ≦ 14, and 0 < y3 ≦ 1.0. Optionally, the electrolytic solution may further satisfy 0.5 ≦ y1 / x ≦ 4.0, 10 ≦ y2 / x ≦ 28, and 0.001 ≦ y3 / x ≦ 2.0. Further optionally, the electrolytic solution may further satisfy 6 ≦ y2 / y1 ≦ 48 and / or 0.036 ≦ x / (y2 + y3) ≦ 0.1.
[0111] In some embodiments, the electrolytic solution further contains a lithium salt and an organic solvent. In the present application, the types of the lithium salt and the organic solvent are not specifically limited and can be selected according to actual needs.
[0112] For example, the lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(oxalato)borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalato)phosphate (LiDFOP), and lithium tetrafluoro(oxalato)phosphate (LiTFOP). Optionally, the lithium salt includes lithium hexafluorophosphate.
[0113] By way of example, the organic solvent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).
[0114] In the embodiment of the secondary battery of the present application, the electrolyte does not exclude other components other than the above components. In some examples, the electrolyte may further include other additives, such as an additive for improving the overcharge performance of the battery, an additive for improving the high temperature performance of the battery, an additive for improving the low temperature power performance of the battery, etc.
[0115] In some embodiments, the mass of the electrolyte may be 10% to 20% of the total mass of the secondary battery. This is advantageous to form a dense and low impedance interfacial film on the surface of the positive electrode active material. And the following situation can be effectively avoided. When the mass fraction of the electrolyte is less than 10%, the electrolyte infiltration of the positive electrode and the negative electrode is low, the interfacial impedance is high, and the impedance increases quickly after cycling, which may cause the secondary battery to exhibit low capacity and poor cycle performance; when the mass fraction of the electrolyte is more than 20%, the interfacial side reaction between the electrolyte and the positive electrode and the electrolyte and the negative electrode increases, the irreversible consumption of active lithium ions increases, and the battery volume expands severely, which may cause the secondary battery to exhibit poor cycle performance.
[0116] The electrolyte may be prepared according to a general method in the art. For example, an electrolyte may be obtained by uniformly mixing components such as an organic solvent, a lithium salt, lithium tetrafluoroborate, optional fluoroethylene carbonate, optional fluorosulfonylimide lithium salt, and optional fluorosulfonic acid lithium salt. There is no particular restriction on the order of addition of each substance. For example, components such as lithium salt, lithium tetrafluoroborate, optional fluoroethylene carbonate, optional fluorosulfonylimide lithium salt, and optional fluorosulfonic acid lithium salt may be added to an organic solvent and uniformly mixed to obtain an electrolyte, or a lithium salt may be added to an organic solvent first, and then components such as lithium tetrafluoroborate, optional fluoroethylene carbonate, optional fluorosulfonylimide lithium salt, and optional fluorosulfonic acid lithium salt may be added to an organic solvent and uniformly mixed to obtain an electrolyte.
[0117] In the present application, each component and its content in the electrolyte may be measured according to a method known in the art, for example, gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), etc.
[0118] It should be noted that when testing the electrolyte of the present application, the electrolyte may be obtained from a secondary battery. An exemplary method for obtaining the electrolyte from a secondary battery includes the following steps: Discharge the secondary battery to a discharge cut-off voltage (for safety reasons, the battery is generally in a fully discharged state), then perform a centrifugal process, and take an appropriate amount of the liquid obtained by the centrifugal process as the electrolyte. The electrolyte may also be obtained directly from the inlet of the secondary battery.
[0119] [Positive plate] The positive electrode plate of the present application includes a positive electrode current collector and a positive electrode film layer located on a surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces facing each other in a thickness direction of the positive electrode current collector, and the positive electrode film layer is on either one or both of the two facing surfaces of the positive electrode current collector.
[0120] The positive electrode current collector may be a metal foil sheet or a composite current collector. An example of the metal foil sheet may be aluminum foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0121] The positive electrode membrane layer generally includes a positive electrode active material, an optional adhesive, and an optional conductive agent. The positive electrode membrane layer is generally formed by applying a positive electrode slurry onto a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode active material, the optional conductive agent, the optional adhesive, and any other components in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP). For example, the adhesive used in the positive electrode membrane layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. By way of example, the conductive agent used in the positive electrode membrane layer may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0122] The positive electrode active material has the molecular formula Li a Ni b Co c M1 d M2 e O f A g The present invention includes a layered material in which
[0123] In some embodiments, the molecular formula is Li a Ni b Co c M1 d M2 e O f A g The layered material represented by formula (I) can be optionally doped with M2 cations, A anions, or simultaneously doped with M2 cations and A anions, so that the crystal structure of the layered material obtained after doping is more stable, and the electrochemical performance, such as cycle performance, rate performance, etc., of the secondary battery can be further improved.
[0124] In some embodiments, A is selected from F. After being doped with F, Li a Ni b Co c M1 d M2 e O f A g The structure is more stable, and the secondary battery can have better cycle performance and rate performance.
[0125] In some embodiments, M1 is selected from Mn.
[0126] In some embodiments, M1 is selected from Al.
[0127] In some embodiments, M1 is selected from the combination of Mn and Al. There is no particular limitation on the molar ratio of Mn and Al, which can be selected according to actual needs.
[0128] In some embodiments, 0.50 ≦ b < 0.98. Optionally, 0.55 ≦ b < 0.98, 0.60 ≦ b < 0.98, 0.65 ≦ b < 0.98, 0.70 ≦ b < 0.98, 0.75 ≦ b < 0.98, or 0.80 ≦ b < 0.98.
[0129] In some embodiments, c = 0.
[0130] In some embodiments, 0 < c < 0.1. Optionally, 0 < c ≦ 0.09, 0 < c ≦ 0.08, 0 < c ≦ 0.07, 0 < c ≦ 0.06, 0 < c ≦ 0.05, 0 < c ≦ 0.04, 0 < c ≦ 0.03, 0 < c ≦ 0.02, or 0 < c ≦ 0.01.
[0131] In some embodiments, 0 < d ≦ 0.45. Optionally, 0 < d ≦ 0.40, 0 < d ≦ 0.35, 0 < d ≦ 0.30, 0 < d ≦ 0.25, 0 < d ≦ 0.20, 0 < d ≦ 0.15, or 0 < d ≦ 0.10.
[0132] In some embodiments, e = 0.
[0133] In some embodiments, 0 < e ≦ 0.5. Optionally, 0 < e ≦ 0.45, 0 < e ≦ 0.40, 0 < e ≦ 0.35, 0 < e ≦ 0.30, 0 < e ≦ 0.25, 0 < e ≦ 0.20, 0 < e ≦ 0.15, 0 < e ≦ 0.10, or 0 < e ≦ 0.05.
[0134] In some embodiments, f = 2, g = 0.
[0135] In some embodiments, f = 0, g = 2.
[0136] In some embodiments, 0 < f < 2, 0 < g < 2, and f + g = 2.
[0137] By way of example, the molecular formula is Li a Ni b Co c M1 d M2 e O fA g The layered material is LiNi 0.7 Mn 0.3 O2, LiNi 0.69 Co 0.01 Mn 0.3 O2, LiNi 0.68 Co 0.02 Mn 0.3 O2, LiNi 0.65 Co 0.05 Mn 0.3 O2, LiNi 0.63 Co 0.07 Mn 0.3 O2, LiNi 0.61 Co 0.09 Mn 0.3 O2.
[0138] Li a Ni b Co c M1 d M2 e O f A gmay be manufactured according to a common method in the art. An exemplary manufacturing method is as follows. A lithium source, a nickel source, a cobalt source, an M1 element precursor, an optional M2 element precursor, and an optional A element precursor are mixed and then sintered to obtain the result. The sintering atmosphere may be an oxygen-containing atmosphere, for example, an air atmosphere or an oxygen atmosphere. The O2 concentration of the sintering atmosphere is, for example, 70% to 100%. The sintering temperature and sintering time may be adjusted according to the actual situation. For example, the lithium source includes, but is not limited to, one or more of lithium oxide (Li2O), lithium phosphate (Li3PO4), lithium dihydrogen phosphate (LiH2PO4), lithium acetate (CH3COOLi), lithium hydroxide (LiOH), lithium carbonate (Li2CO3), and lithium nitrate (LiNO3). For example, the nickel source includes, but is not limited to, one or more of nickel sulfate, nickel nitrate, nickel chloride, nickel oxalate, and nickel acetate. For example, the cobalt source includes, but is not limited to, one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate, and cobalt acetate. For example, the M1 element precursor includes, but is not limited to, one or more of oxide, nitrate, carbonate, hydroxide, and acetate of the M1 element. For example, the M2 element precursor includes, but is not limited to, one or more of oxide, nitrate, carbonate, hydroxide, and acetate of the M2 element. For example, the A element precursor includes, but is not limited to, one or more of ammonium fluoride, lithium fluoride, hydrogen fluoride, ammonium chloride, lithium chloride, hydrogen chloride, ammonium nitrate, ammonium nitrite, ammonium carbonate, ammonium hydrogen carbonate, ammonium phosphate, phosphoric acid, ammonium sulfate, ammonium hydrogen sulfate, ammonium hydrogen sulfite, ammonium sulfite, ammonium hydrogen sulfide, hydrogen sulfide, lithium sulfide, ammonium sulfide, and elemental sulfur.
[0139] In some embodiments, Li a Ni b Co c M1 d M2 e O f Ag The surface of the positive electrode active material may further have a coating layer, for example, a carbon coating layer. The carbon coating layer is advantageous in stabilizing the surface of the positive electrode active material, further reducing the charge transfer impedance of the positive electrode active material, and reducing the diffusion resistance of lithium ions in the bulk phase of the positive electrode active material. Optionally, the carbon coating layer includes amorphous carbon, for example, soft carbon, hard carbon, or a combination thereof.
[0140] In some embodiments, the positive electrode active material is Li a Ni b Co c M1 d M2 e O f A g For example, the positive electrode active material may further include one or more of lithium-containing phosphates and their modifying compounds. For example, the lithium-containing phosphates may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and each of the modifying compounds.
[0141] In some embodiments, the molecular formula is Li a Ni b Co c M1 d M2 e O f A g The mass percentage of the layered material is 80% to 99%. For example, a Ni b Co c M1 d M2 e O f A g The weight percentage of the layered material having the molecular formula Li is 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or any range therein.a Ni b Co c M1 d M2 e O f A g The mass percentage of the layered material is 85%-99%, 90%-99%, 95%-99%, 80%-98%, 85%-98%, 90%-98%, 95%-98%, 80%-97%, 85%-97%, 90%-97%, or 95%-97%.
[0142] [Negative plate] The secondary battery according to the present application further includes a negative electrode plate. In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer located on a surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces facing each other in a thickness direction thereof, and the negative electrode film layer is on either one or both of the two facing surfaces of the negative electrode current collector.
[0143] The negative electrode current collector may be a metal foil sheet or a composite current collector. An example of the metal foil sheet may be copper foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0144] The negative electrode membrane layer generally includes a negative electrode active material, an optional adhesive, an optional conductive agent, and other optional auxiliary agents. The negative electrode membrane layer is generally formed by applying a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is generally formed by dispersing the negative electrode active material, the optional conductive agent, the optional adhesive, and other optional auxiliary agents in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water. For example, the adhesive used in the negative electrode membrane layer may include one or more of styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). For example, the conductive agent used in the negative electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, ketjen black, carbon spots, carbon nanotubes, graphene, and carbon nanofibers. Other optional auxiliary agents may include thickeners (e.g., sodium carboxymethylcellulose CMC-Na), PTC thermistor materials, etc.
[0145] The negative electrode active material may be a negative electrode active material for secondary batteries well known in the art. For example, the negative electrode active material may include one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicone-based material, tin-based material, and lithium titanate. The silicone-based material may include one or more of silicone simple substance, silicone oxide, silicone carbon composite, silicone nitrogen composite, and silicone alloy material. The tin-based material may include one or more of tin simple substance, tin oxide, and tin alloy material. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials for secondary batteries may be used. These negative electrode active materials may be used alone or in combination of two or more.
[0146] [Separator] The secondary battery according to the present application may further include a separator. The separator is disposed between the positive electrode plate and the negative electrode plate to serve as an insulator. The present application is not particularly limited to the type of the separator, and any known membrane having a porous structure with good chemical and mechanical stability may be selected.
[0147] In some embodiments, the separator may be made of one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a monolayer film or a multilayer composite film. When the separator is a multilayer composite film, the materials of each layer may be the same or different.
[0148] In some embodiments, the positive plate, the separator and the negative plate can be wound and / or stacked to form an electrode assembly.
[0149] In some embodiments, the secondary battery may include an exterior body. The exterior body may be used to package the electrode assembly and the electrolyte. The exterior body of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior body of the secondary battery may be a pouch, such as a bag-shaped pouch. The material of the pouch may be one or more of plastics, such as polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0150] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular or any other shape. Figure 1 shows a secondary battery 5 with a rectangular structure as an example.
[0151] In some embodiments, as shown in FIG. 2, the exterior body may include a case 51 and a cover plate 53. The case 51 may include a bottom plate and a side plate connected on the bottom plate, and the bottom plate and the side plate surround and form a receiving cavity. The case 51 has an opening communicating with the receiving cavity, and the cover plate 53 is provided to cover the opening and close the receiving cavity. The positive electrode plate, the negative electrode plate and the separator may form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the receiving cavity. An electrolyte is permeated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to demand.
[0152] In some embodiments of the present application, the secondary battery according to the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number can be adjusted based on the application and capacity of the battery module.
[0153] Fig. 3 is a schematic diagram of an example battery module 4. As shown in Fig. 3, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed with fasteners.
[0154] Optionally, the battery module 4 may further include a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.
[0155] In some embodiments, the above battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted based on the application and capacity of the battery pack.
[0156] 4 and 5 are schematic diagrams of an example battery pack 1. As shown in FIG. 4 and FIG. 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 is provided to cover the lower housing 3 and is used to form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box according to any manner.
[0157] Manufacturing method An embodiment of the present application further provides a method for manufacturing a secondary battery, the method including at least step 1 and step 2.
[0158] Step 1 of assembling a positive electrode plate, a separator, a negative electrode plate, and an electrolyte into a secondary battery, the positive electrode plate including a positive electrode current collector and a positive electrode film layer located on a surface of the positive electrode current collector, the positive electrode film layer having a molecular formula of Li a Ni b Co c M1 d M2 e O f A gIt contains a layered material, where M1 is selected from Mn, Al, or a combination thereof, M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te, and W, A is selected from one or more of F, N, P, and S, 0.8 ≦ a ≦ 1.2, 0 < b < 0.98, 0 ≦ c < 0.1, 0 < d < 0.5, 0 ≦ e ≦ 0.5, 0 ≦ f ≦ 2, 0 ≦ g ≦ 2, b + c + d + e = 1, f + g = 2. The electrolyte contains lithium tetrafluoroborate, optional fluoroethylene carbonate, optional lithium fluorosulfonylimide salt, and optional lithium fluorosulfonate salt. The mass percentage of lithium tetrafluoroborate in the electrolyte is x%, the mass percentage of fluoroethylene carbonate in the electrolyte is y1%, the mass percentage of lithium fluorosulfonylimide salt in the electrolyte is y2%, and the mass percentage of lithium fluorosulfonate salt in the electrolyte is y3%, all calculated based on the total mass of the electrolyte, where x > 0, y1 ≧ 0, y2 ≧ 0, y3 ≧ 0.
[0159] Step 2, from the secondary battery obtained in Step 1, select a secondary battery that satisfies 0.05 ≦ c + x / 10 ≦ 0.15.
[0160] When the secondary battery satisfies x > 0 and 0.05 ≦ c + x / 10 ≦ 0.15, it can stabilize the crystal structure of the low-cobalt or cobalt-free cathode active material and improve the diffusion rate of lithium ions inside. Therefore, the secondary batteries obtained by the manufacturing method of this application can all have significantly improved cycle performance, good storage performance, and kinetic performance.
[0161] In some embodiments, the method further includes the step of selecting a secondary battery that satisfies 0 < x ≦ 1.0 and 0.05 ≦ c + x / 10 ≦ 0.15 from the secondary batteries obtained in Step 2. At this time, the manufactured secondary batteries have further improved cycle performance. Optionally, the secondary battery satisfies 0.05 ≦ c + x / 10 ≦ 0.12.
[0162] In some embodiments, the method further includes a step of selecting a secondary battery that satisfies 25 ≦ P / (c + x / 10) ≦ 65 from the secondary batteries obtained in step 2, where P g / cm 3 represents the consolidation density of the positive electrode plate. At this time, on the premise that the manufactured secondary battery has significantly improved cycle performance and high energy density, it can have improved power performance. Optionally, the secondary battery satisfies 30 ≦ P / (c + x / 10) ≦ 50.
[0163] In some embodiments, the method further includes a step of selecting a secondary battery that satisfies at least one of the following conditions (1) to (3) from the secondary batteries obtained in step 2.
[0164] (1) 0 < y1 ≦ 2.5, 0.5 ≦ y1 / x ≦ 4.0, optionally 0.5 ≦ y1 / x ≦ 2.0, (2) 0 < y2 ≦ 14, 1 ≦ y2 / x ≦ 28, (3) 0 < y3 ≦ 1.0, 0.001 ≦ y3 / x ≦ 2.0, optionally 0.001 ≦ y3 / x ≦ 1.0.
[0165] At this time, the manufactured secondary battery has at least one of further improved cycle performance, storage performance, rate performance, low-temperature performance, and high-temperature performance.
[0166] In some embodiments, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≦ 15, 0 < y1 ≦ 2.5, 0 < y2 ≦ 14, 0 < y3 ≦ 1.0, 0.5 ≦ y1 / x ≦ 4.0, 1 ≦ y2 / x ≦ 28, 0.001 ≦ y3 / x ≦ 2.0, 0.5 ≦ y2 / y1 ≦ 48 from the secondary batteries obtained in step 2. At this time, the overall performance of the manufactured secondary battery is further improved.
[0167] Optionally, when 0 < b ≤ 0.7, the method further includes the step of selecting a secondary battery obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10.
[0168] Optionally, when 0.7 ≤ b < 0.98, the method further includes the step of selecting a secondary battery obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 5 ≤ y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 10 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 6 ≤ y2 / y1 ≤ 48.
[0169] In some embodiments, the method further includes the step of selecting a secondary battery obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 14, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 28, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 48, 0.036 ≤ x / (y2 + y3) ≤ 1.0. At this time, the comprehensive performance of the manufactured secondary battery is further improved.
[0170] Optionally, when 0 < b ≤ 0.7, the method further includes the step of selecting a secondary battery obtained in step 2 that satisfies 0 < y1 + y2 + y3 ≤ 15, 0 < y1 ≤ 2.5, 0 < y2 ≤ 5, 0 < y3 ≤ 1.0, 0.5 ≤ y1 / x ≤ 4.0, 1 ≤ y2 / x ≤ 10, 0.001 ≤ y3 / x ≤ 2.0, 0.5 ≤ y2 / y1 ≤ 10, 0.1 ≤ x / (y2 + y3) ≤ 1.0.
[0171] Optionally, when 0.7 ≦ b < 0.98, the method further includes a step of selecting a secondary battery that satisfies 0 < y1 + y2 + y3 ≦ 15, 0 < y1 ≦ 2.5, 5 ≦ y2 ≦ 14, 0 < y3 ≦ 1.0, 0.5 ≦ y1 / x ≦ 4.0, 10 ≦ y2 / x ≦ 28, 0.001 ≦ y3 / x ≦ 2.0, 6 ≦ y2 / y1 ≦ 48, and 0.036 ≦ x / (y2 + y3) ≦ 0.1 from the secondary battery obtained in Step 2.
[0172] Power consumption device Embodiments of the present application further provide a power consumption device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack may be used as a power source for the power consumption device or as an energy storage unit of the power consumption device. The power consumption device may be a mobile device (such as a mobile phone, laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, hybrid electric vehicle, plug-in hybrid electric vehicle, electric bicycle, electric scooter, electric golf cart, electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc., but is not limited thereto.
[0173] As the power consumption device, a secondary battery, battery module, or battery pack can be selected according to the requirements in its use.
[0174] FIG. 6 is a schematic diagram of a power consumption device as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the requirements for high power and high energy density of the power consumption device, a battery pack or a battery module can be adopted.
[0175] Another example of the power consumption device may be a mobile phone, a tablet computer, a laptop computer, etc. The power consumption device generally requires weight reduction, and a secondary battery can be adopted as a power source.
[0176] Examples The following examples are provided to more specifically describe the contents disclosed in this application, and these examples are used merely for illustrative purposes, and it is obvious to those skilled in the art that various modifications and changes can be made within the scope of the contents disclosed in this application. Unless otherwise indicated, all parts, percentages, and ratios reported in the following examples are all by weight, all reagents used in the examples are all commercially available or can be synthesized by common methods, and can be used directly without further processing, and all equipment used in the examples can be commercially available.
[0177] Example 1-1 Positive electrode plate manufacturing Positive electrode active material LiNi 0.65 Co 0.05 Mn 0.3 O2, carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive were mixed in a mass ratio of 97.5:1.4:1.1 in an appropriate amount of NMP solvent by thorough stirring to form a uniform positive electrode slurry, which was then uniformly coated on the surface of the aluminum foil of the positive electrode current collector, dried, and cold pressed to obtain a positive electrode plate. The compaction density of the positive electrode plate was 3.5 g / cm. 3 It is.
[0178] Negative plate manufacturing The negative electrode active material graphite, the adhesive styrene butadiene rubber (SBR), the thickener sodium carboxymethylcellulose (CMC-Na), and the conductive agent carbon black (Super P) were mixed in a mass ratio of 96.2:1.8:1.2:0.8 in an appropriate amount of deionized water as a solvent and stirred thoroughly to form a uniform negative electrode slurry. The negative electrode slurry was then evenly coated on the surface of the copper foil of the negative electrode current collector, and after drying and cold pressing, a negative electrode plate was obtained.
[0179] Separator A porous polyethylene (PE) membrane was employed as the separator.
[0180] Electrolyte production Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and LiPF6 and LiBF4 are uniformly dissolved in the organic solvent to obtain an electrolyte, in which the mass percentage of LiPF6 is 12.5% and the mass percentage of LiBF4 is 0.1% based on the total mass of the electrolyte.
[0181] Secondary battery manufacturing A positive electrode plate, a separator, and a negative electrode plate were stacked in this order and wound to obtain an electrode assembly, which was then placed in an outer casing, and the above-mentioned electrolyte was added. A secondary battery was obtained through processes such as packaging, standing, chemical formation, and aging. The mass of the electrolyte was 15% of the total mass of the secondary battery.
[0182] Examples 1-2 to 1-16 and Comparative Examples 1-1 to 1-7 The manufacturing method of the secondary battery is similar to that of Example 1, but the difference is that the type of positive electrode active material and the manufacturing parameters of the electrolyte are adjusted, and the specific parameters are as shown in Table 1. " / " indicates that the corresponding component is not added to the electrolyte.
[0183] Test part (1) Room temperature cycle performance test of secondary batteries At 25°C, the secondary battery was charged to 4.3V at a constant current of 1C, and then charged at a constant voltage until the current became 0.05C. At this time, the secondary battery was in a fully charged state, and the charge capacity at this time was recorded and set as the first charge capacity. The secondary battery was left to stand for 5 minutes, and then discharged to 2.8V at a constant current of 1C. This was one cycle charge / discharge process, and the discharge capacity at this time was recorded and set as the first discharge capacity. The secondary battery was subjected to a cycle charge / discharge test using the above method, and the discharge capacity after each cycle was recorded. The capacity retention rate (%) of the secondary battery at 25°C after 600 cycles = discharge capacity after 600 cycles / first discharge capacity × 100%.
[0184] (2) High-temperature cycle performance test of secondary batteries At 45°C, the secondary battery was charged to 4.3V at a constant current of 1C, and then charged at a constant voltage until the current became 0.05C. At this time, the secondary battery was in a fully charged state, and the charge capacity at this time was recorded and set as the first charge capacity. The secondary battery was left to stand for 5 minutes, and then discharged to 2.8V at a constant current of 1C. This was one cycle charge / discharge process, and the discharge capacity at this time was recorded and set as the first discharge capacity. The secondary battery was subjected to a cycle charge / discharge test using the above method, and the discharge capacity after each cycle was recorded. The capacity retention rate (%) of the secondary battery at 45°C after 600 cycles = discharge capacity after 600 cycles / first discharge capacity × 100%.
[0185] (3) Initial DC internal resistance test for secondary batteries At 25°C, the secondary battery was charged to 4.3V at a constant current of 1C, and then charged at a constant voltage until the current reached 0.05C, at which point the secondary battery was in a fully charged state. The secondary battery was discharged at a constant current of 0.5C to adjust the secondary battery to 50% SOC, at which point the voltage of the secondary battery was recorded as U1, and the secondary battery was discharged at a constant current of 4C I1 for 30 seconds, scored at 0.1 seconds, and the voltage at the end of discharge was recorded as U2. The initial DC internal resistance of the secondary battery can be expressed using the discharge DC internal resistance when the secondary battery is at 50% SOC, as follows: initial DC internal resistance of the secondary battery (mΩ) = (U1-U2) / I1.
[0186] (4) High-temperature storage performance test for secondary batteries At 60℃, the secondary battery was charged to 4.3V at a constant current of 1C, and then charged at a constant voltage until the current reached 0.05C, at which point the volume of the secondary battery was tested using the drainage method and recorded as V0, the secondary battery was placed in a thermostatic box at 60℃ and stored for 30 days, after which it was taken out, at which point the volume of the secondary battery was tested using the drainage method and recorded as V1. The volume expansion rate (%) of the secondary battery after 30 days of storage at 60℃ = [(V1-V0) / V0] × 100%.
[0187] (5) Secondary battery self-discharge rate test At 25°C, the secondary battery was charged to 70% SOC, and the open circuit voltage of the secondary battery at this time was tested and recorded as OCV1. The secondary battery was placed in a thermostatic box at 25°C and stored for 3 months, then removed and the open circuit voltage of the secondary battery was tested again and recorded as OCV2. The self-discharge rate of the secondary battery stored for 3 months at 25°C = [(OCV1-OCV2) / OCV1] x 100%. The lower the self-discharge rate of the secondary battery, the higher the capacity performance and safety performance.
[0188] (6) Low-temperature performance test of secondary batteries At -10°C, the secondary battery was charged to 4.3V at a constant current of 0.2C, and then charged at a constant voltage until the current became 0.05C. At this time, the secondary battery was in a fully charged state, and the charge capacity at this time was recorded and set as the first charge capacity. The secondary battery was left to stand for 30 minutes, and then discharged to 2.8V at a constant current of 0.2C. This was one cycle charge / discharge process, and the discharge capacity at this time was recorded and set as the first discharge capacity. The secondary battery was subjected to a cycle charge / discharge test by the above method, and the discharge capacity after each cycle was recorded. The capacity retention rate (%) of the secondary battery at -10°C after 200 cycles = discharge capacity after 200 cycles / first discharge capacity × 100%.
[0189] Table 1 shows the performance test results of Examples 1-1 to 1-16 and Comparative Examples 1-1 to 1-7.
[0190] As can be seen from the test results in Table 1, when the electrolyte contains lithium tetrafluoroborate, and the mass percentage of lithium tetrafluoroborate x% and the content of cobalt element c in the low-cobalt or cobalt-free positive electrode active material are such that x>0 and 0.05≦c+x / 10≦0.15, the secondary battery has significantly improved cycle performance and good storage performance and dynamic performance. When the electrolyte does not contain lithium tetrafluoroborate, or the content of lithium tetrafluoroborate is too high or too low and does not satisfy 0.05≦c+x / 10≦0.15, the cycle performance of the low-cobalt or cobalt-free secondary battery cannot be effectively improved, and the internal resistance of the secondary battery is high.
[0191] As can be seen from the test results in Table 1, the compaction density of the positive plate, P g / cm 3 When the mass percentage of lithium tetrafluoroborate x% and the content c of the cobalt element in the low-cobalt or cobalt-free positive electrode active material further satisfy 25≦P / (c+x / 10)≦65, the secondary battery can have a lower internal resistance.
[0192] The inventors further studied the effects of components other than lithium tetrafluoroborate in the electrolyte on the performance of the secondary battery.
[0193] The manufacturing methods of the secondary batteries of Examples 2-1 to 2-20 are similar to those of Examples 1-3, but the manufacturing parameters of the electrolyte are adjusted, and the specific parameters are as shown in Table 2. " / " indicates that the corresponding component is not added to the electrolyte.
[0194] As can be seen from the test results in Table 2, when the electrolyte solutions of Examples 2-1 to 2-20 further contain one or more of fluoroethylene carbonate (FEC), lithium bis(fluorosulfonyl)imide (LiFSI) and lithium fluorosulfonate, it contributes to further improving the overall performance of the secondary battery.
[0195] As can be seen from the summary of the test results of Examples 2-9, 1-3, 2-1 to 2-6, when the electrolyte solution of Examples 1-3 is used as the base, and fluoroethylene carbonate, lithium bis(fluorosulfonyl)imide and lithium fluorosulfonate are added at the same time, it contributes to obtaining a secondary battery with better overall performance.
[0196] As can be seen from the summary of the test results of Examples 2-7 to 2-20, when the mass percentage y1% of fluoroethylene carbonate, the mass percentage y2% of lithium bis(fluorosulfonyl)imide and the mass percentage y3% of lithium fluorosulfonate are adjusted to simultaneously satisfy 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦48, 0.036≦x / (y2+y3)≦1.0, it contributes to obtaining a secondary battery with better overall performance. A possible reason is that at this time, an inorganic / organic composite interface film with excellent performance can be formed on both the positive and negative electrodes.
[0197] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is an example, and any embodiment having substantially the same configuration as the technical idea and achieving the same effect within the scope of the technical proposal of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application, within the scope of the purpose of the present application.
[0198] JPEG2024540706000002.jpg213131 JPEG2024540706000003.jpg217107
[0199] JPEG2024540706000004.jpg226127JPEG2024540706000005.jpg22793 [Explanation of symbols]
[0200] In the drawings, which are not necessarily drawn to scale, the reference numerals are explained as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 case, 52 electrode assembly, 53 cover plate.
Claims
1. A secondary battery including an electrolyte and a positive electrode plate, The positive electrode plate includes a positive electrode current collector and a positive electrode film layer located on a surface of the positive electrode current collector, the positive electrode film layer having a molecular formula of Li a Ni b Co c M1 d M2 e O f A g wherein M1 is selected from Mn, Al or combinations thereof; M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te and W; A is selected from one or more of F, N, P and S; and wherein 0.8≦a≦1.2, 0<b<0.98, 0≦c<0.1, 0<d<0.5, 0≦e≦0.5, 0≦f≦2, 0≦g≦2, b+c+d+e=1, f+g=2; The electrolyte contains lithium tetrafluoroborate, a mass percentage of the lithium tetrafluoroborate in the electrolyte is x % based on a total mass of the electrolyte, and the secondary battery satisfies x>0 and 0.05≦c+x / 10≦0.
15.
2. 0.05≦c+x / 10≦0.12, and / or The secondary battery according to claim 1 , wherein 0<x≦1.
0.
3. The compaction density of the positive electrode plate is P g / cm 3 and the secondary battery satisfies 25≦P / (c+x / 10)≦65, optionally 30≦P / (c+x / 10)≦50; 3. The secondary battery according to claim 1 or 2, optionally wherein P is 3.3 to 3.
6.
4. The secondary battery according to any one of claims 1 to 3, wherein the electrolytic solution further contains one or more of fluoroethylene carbonate, a lithium fluorosulfonylimide salt, and a lithium fluorosulfonate salt, the mass percentage of the fluoroethylene carbonate in the electrolytic solution is y1%, the mass percentage of the lithium fluorosulfonylimide salt in the electrolytic solution is y2%, and the mass percentage of the lithium fluorosulfonate in the electrolytic solution is y3%, all of which are calculated based on the total mass of the electrolytic solution, and the electrolytic solution satisfies y1 ≧ 0, y2 ≧ 0, y3 ≧ 0, and 0 < y1 + y2 + y3 ≦ 15.
5. The molecular formula of the lithium fluorosulfonylimide salt is LiN(SO 2 R 1 ) (SO 2 R 2 ) and R 1 , R 2 are each independently F or C n F 2n+1 wherein n is an integer from 1 to 10; and optionally, the fluorosulfonylimide lithium salt comprises lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonylimide, or a combination thereof; and / or The molecular formula of the lithium fluorosulfonate is LiSO 3 R 3 and R 3 represents F, a partially fluorinated or fully fluorinated C1-C10 alkyl group, and optionally, the lithium fluorosulfonate salt comprises lithium fluorosulfonate, lithium trifluoromethanesulfonate, or a combination thereof.
6. The mass percentage y1% of the fluoroethylene carbonate in the electrolyte solution is 0<y1≦2.5, optionally 0<y1≦2.0, and / or The secondary battery according to claim 4 or 5, satisfying 0.5≦y1 / x≦4.0, optionally 0.5≦y1 / x≦2.
0.
7. The mass percentage y2% of the fluorosulfonylimide lithium salt in the electrolyte solution is 0<y2≦14, and / or The secondary battery according to any one of claims 4 to 6, wherein 1≦y2 / x≦28 is satisfied.
8. When 0<b≦0.7, the mass percentage y2% of the fluorosulfonylimide lithium salt in the electrolyte solution satisfies 0<y2≦5 and / or 1≦y2 / x≦10, optionally 0<y2≦2.5, optionally 1≦y2 / x≦5; 8. The secondary battery according to claim 7, wherein, when 0.7≦b<0.98, the mass percentage y2% of the fluorosulfonylimide lithium salt in the electrolyte solution satisfies 5≦y2≦14 and / or 10≦y2 / x≦28, optionally 8≦y2≦14, optionally 16≦y2 / x≦28.
9. The mass percentage y3% of the lithium fluorosulfonate salt in the electrolyte solution is 0<y3≦1.0, optionally 0<y3≦0.5, and / or The secondary battery according to any one of claims 4 to 8, wherein 0.001≦y3 / x≦2.0, optionally 0.001≦y3 / x≦1.0, is satisfied.
10. The electrolyte further comprises fluoroethylene carbonate, a fluorosulfonylimide lithium salt, and a fluorosulfonic acid lithium salt, and the electrolyte satisfies 0<y1≦2.5, 0<y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, 0.001≦y3 / x≦2.0, and 0.5≦y2 / y1≦48; Optionally, when 0<b≦0.7, the electrolyte satisfies 0<y1≦2.5, 0<y2≦5, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦10, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦10; Optionally, when 0.7≦b<0.98, the electrolyte satisfies 0<y1≦2.5, 5≦y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 10≦y2 / x≦28, 0.001≦y3 / x≦2.0, and 6≦y2 / y1≦48. The secondary battery according to claim 4 or 5.
11. The electrolyte further comprises fluoroethylene carbonate, a fluorosulfonylimide lithium salt, and a fluorosulfonic acid lithium salt, and the electrolyte satisfies 0<y1≦2.5, 0<y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦48, and 0.036≦x / (y2+y3)≦1.0; Optionally, when 0<b≦0.7, the electrolyte satisfies 0<y1≦2.5, 0<y2≦5, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦10, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦10, 0.1≦x / (y2+y3)≦1.0; Optionally, when 0.7≦b<0.98, the electrolyte solution satisfies 0<y1≦2.5, 5≦y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 10≦y2 / x≦28, 0.001≦y3 / x≦2.0, 6≦y2 / y1≦48, 0.036≦x / (y2+y3)≦0.
1. The secondary battery according to claim 4 or 5.
12. The secondary battery according to any one of claims 1 to 11, wherein 0<c<0.
1.
13. The secondary battery according to any one of claims 1 to 11, wherein c = 0.
14. Based on the total mass of the positive electrode film layer, the molecular formula is Li a Ni b Co c M1 d M2 e O f A g 14. The secondary battery of claim 1, wherein the mass percentage of the layered material which is is between 80% and 99%, optionally between 85% and 99%.
15. The secondary battery according to any one of claims 1 to 14, further comprising a mass of the electrolyte of 10% to 20% of a total mass of the secondary battery.
16. A method for manufacturing a secondary battery, comprising at least Step 1 of assembling a positive electrode plate, a separator, a negative electrode plate, and an electrolyte into a secondary battery, The positive electrode plate includes a positive electrode current collector and a positive electrode film layer located on a surface of the positive electrode current collector, the positive electrode film layer having a molecular formula of Li a Ni b Co c M1 d M2 e O f A g wherein M1 is selected from Mn, Al or combinations thereof; M2 is selected from one or more of Si, Ti, Mo, V, Ge, Se, Zr, Nb, Ru, Pd, Sb, Ce, Te and W; A is selected from one or more of F, N, P and S; and 0.8≦a≦1.2, 0<b<0.98, 0≦c<0.1, 0<d<0.5, 0≦e≦0.5, 0≦f≦2, 0≦g≦2, b+c+d+e=1, f+g=2; step 1, the electrolyte comprising lithium tetrafluoroborate, optional fluoroethylene carbonate, optional lithium fluorosulfonylimide salt, and optional lithium fluorosulfonate salt, wherein the weight percentage of the lithium tetrafluoroborate in the electrolyte is x%, the weight percentage of the fluoroethylene carbonate in the electrolyte is y1%, the weight percentage of the lithium fluorosulfonylimide salt in the electrolyte is y2%, and the weight percentage of the lithium fluorosulfonate salt in the electrolyte is y3%, all calculated based on a total weight of the electrolyte, and wherein x>0, y1≧0, y2≧0, and y3≧0; and step 2 of selecting secondary batteries that satisfy 0.05≦c+x / 10≦0.15 from the secondary batteries obtained in step 1.
17. The method according to claim 16 , further comprising the step of selecting secondary batteries that satisfy 0<x≦1.0 and 0.05≦c+x / 10≦0.15 from the secondary batteries obtained in step 2.
18. The method further includes a step of selecting secondary batteries that satisfy 25≦P / (c+x / 10)≦65 from the secondary batteries obtained in step 2, and P g / cm 3 The method of claim 16, wherein: represents the packed density of the positive plate.
19. The method further includes a step of selecting secondary batteries that satisfy the following conditions from the secondary batteries obtained in step 2: 0<y1+y2+y3≦15, 0<y1≦2.5, 0<y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦48; Optionally, when 0<b≦0.7, further comprising the step of selecting secondary batteries that satisfy 0<y1+y2+y3≦15, 0<y1≦2.5, 0<y2≦5, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦10, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦10 from the secondary batteries obtained in step 2; Optionally, when 0.7≦b<0.98, the method of claim 16 further comprises a step of sorting secondary batteries that satisfy 0<y1+y2+y3≦15, 0<y1≦2.5, 5≦y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 10≦y2 / x≦28, 0.001≦y3 / x≦2.0, and 6≦y2 / y1≦48 from the secondary batteries obtained in step 2.
20. The method further includes a step of selecting secondary batteries that satisfy the following conditions from the secondary batteries obtained in step 2: 0<y1+y2+y3≦15, 0<y1≦2.5, 0<y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦28, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦48, 0.036≦x / (y2+y3)≦1.0; Optionally, when 0<b≦0.7, further comprising the step of selecting secondary batteries that satisfy 0<y1+y2+y3≦15, 0<y1≦2.5, 0<y2≦5, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 1≦y2 / x≦10, 0.001≦y3 / x≦2.0, 0.5≦y2 / y1≦10, 0.1≦x / (y2+y3)≦1.0 from the secondary batteries obtained in step 2; Optionally, the method of claim 16 further comprises a step of sorting secondary batteries that satisfy the following conditions from the secondary batteries obtained in step 2 when 0.7≦b<0.98: 0<y1+y2+y3≦15, 0<y1≦2.5, 5≦y2≦14, 0<y3≦1.0, 0.5≦y1 / x≦4.0, 10≦y2 / x≦28, 0.001≦y3 / x≦2.0, 6≦y2 / y1≦48, 0.036≦x / (y2+y3)≦0.
1.
21. A battery module comprising the secondary battery according to any one of claims 1 to 15, or a secondary battery obtained by the method according to any one of claims 16 to 20.
22. A battery pack comprising the secondary battery according to any one of claims 1 to 15, a secondary battery obtained by the method according to any one of claims 16 to 20, or a battery module according to claim 21.
23. A power consuming device comprising at least one of the secondary battery according to any one of claims 1 to 15, the secondary battery obtained by the method according to any one of claims 16 to 20, the battery module according to claim 21, and the battery pack according to claim 22.
Citation Information
Patent Citations
Non-aqueous electrolyte and lithium ion battery
CN107017433A
Lithium ion battery electrolyte and lithium ion battery
CN111048840A
Electrolyte functional additive for lithium ion battery, lithium ion battery electrolyte and lithium ion battery
CN111509298A
Nonaqueous electrolyte secondary battery and method of manufacturing same
JP2007053083A
Nonaqueous electrolyte secondary battery and method for manufacturing the same
JP2017152223A