Polybutylene terephthalate resin composition, its method of manufacture and molded article containing same
The polybutylene terephthalate resin composition addresses the trade-off between solidification speed and impact strength by using specific resin ratios and additives, enhancing both properties and product quality.
Patent Information
- Application Number
- JP2023573284
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Existing polybutylene terephthalate resin compositions face a trade-off between injection solidification speed and impact strength, leading to decreased impact strength when increasing solidification rate and potential cracks in thinner products.
A polybutylene terephthalate resin composition comprising specific ratios of polybutylene terephthalate resins with varying intrinsic viscosities, carboxy-reactive epoxy resin, polybutadiene rubber, and injection solidification accelerators, optimized for balanced mechanical properties, fluidity, and heat resistance.
Simultaneously improves injection solidification rate and impact strength, ensuring excellent product reliability and appearance quality while maintaining physical property balance.
Smart Images

Figure 2024541157000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0124293 dated September 29, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to a polybutylene terephthalate resin composition, a manufacturing method thereof, and a molded article containing the same. More specifically, the present invention relates to a polybutylene terephthalate resin composition that can simultaneously improve injection solidification speed and impact strength, which are in a trade-off relationship depending on the change in raw materials used, and can provide excellent product reliability and appearance quality by satisfying a balance of physical properties such as mechanical properties, fluidity, and heat resistance, and a manufacturing method thereof and a molded article containing the same. [Background technology]
[0003] As a material for automobile parts, a method of increasing the crystallinity of polyester resin by using organic / inorganic injection solidification accelerators to improve the injection solidification speed is widely used.
[0004] However, there is a drawback in that the impact strength is reduced because the degree of crystallinity is increased by improving the solidification speed.
[0005] Furthermore, in recent years, there has been a trend towards smaller and thinner electronic components, which require higher impact strength than before, so techniques for increasing the degree of crystallinity have led to further problems, such as cracks occurring in the products.
[0006] Therefore, when a reinforcing agent is added to reinforce the impact strength, the impact strength is improved and the problem of cracks is solved, but the injection solidification speed is significantly reduced, and there is a trade-off between the injection solidification speed and the impact strength.
[0007] Therefore, there is a need to develop a material for automotive interiors that can overcome this trade-off relationship and efficiently improve both the injection solidification speed and impact strength at the same time. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 2019-156954 (Publication date: 2019.09.19) Summary of the Invention [Problem to be solved by the invention]
[0009] In order to solve the above problems of the conventional technology, the present invention aims to provide a polybutylene terephthalate resin composition that is economical since it can be used as an unpainted product and can reduce the cost by changing the material used, while simultaneously improving the injection solidification speed and impact strength, which are in a trade-off relationship, and satisfying the balance of physical properties such as mechanical properties, fluidity, and heat resistance, thereby providing excellent product reliability and appearance quality.
[0010] Another object of the present invention is to provide a molded article using the polybutylene terephthalate resin composition.
[0011] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]
[0012] In order to achieve the above object, the present invention provides 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less; 0.01 to 10% by weight of a carboxy-reactive epoxy resin; The present invention provides a polybutylene terephthalate resin composition comprising 0.01 to 10% by weight of polybutadiene rubber.
[0013] The polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less may contain a polybutylene terephthalate resin having an intrinsic viscosity of less than 0.9 and a polybutylene terephthalate resin having an intrinsic viscosity of more than 0.9 and 1.05 or less in a weight ratio of 30:70 to 60:40.
[0014] The polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 may contain 29 to 55% by weight of a polybutylene terephthalate resin having an intrinsic viscosity of more than 1.05 and not more than 1.5, relative to 100% by weight of the total amount of all components constituting the polybutylene terephthalate resin composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives).
[0015] The carboxy-reactive epoxy resin may be one or more selected from ethylene-n-butyl acrylate-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-acrylic acid ester-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer, ethylene-dimethacrylate-glycidyl methacrylate copolymer, ethylene-acrylate-glycidyl methacrylate copolymer, and ethylene-vinyl acetate-glycidyl methacrylate copolymer.
[0016] The carboxy-reactive epoxy resin may contain 1 to 15% by weight of units derived from glycidyl methacrylate.
[0017] The polybutadiene rubber may have a bulk density of at least 0.25 g / cc as measured in accordance with ASTM D1895.
[0018] The polybutadiene rubber may have an Izod impact strength (-30°C, 1 / 4" thickness) of 10 kg / cm.cm or more, measured in accordance with ASTM D256, and an Izod impact strength (23°C, 1 / 4" thickness) of 50 kg / cm.cm or more.
[0019] The polybutadiene rubber may have a particle size of 3% or less, based on 100% of all particles, that is, particles passing through a #20 mesh.
[0020] The polybutylene terephthalate resin composition may include an injection solidification accelerator, and specific examples thereof include inorganic injection solidification accelerators such as talc, wollastonite, and mica, or ethylene acrylate acid-based compounds.
[0021] The injection solidification accelerator may be contained in an amount of 0.01 to 1% by weight relative to 100% by weight of the total amount of all components (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives) constituting the polybutylene terephthalate resin composition.
[0022] The polybutylene terephthalate resin composition may contain one or more additives selected from a lubricant, an antioxidant, and a colorant.
[0023] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: 29 to 55% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5; 0 to 68% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05; 0 to 50% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9; 0.01 to 10% by weight of a carboxy-reactive epoxy resin; 0.01 to 10% by weight of polybutadiene rubber, The polybutylene terephthalate resin composition contains 0.01 to 1% by weight of an injection solidification accelerator.
[0024] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: i) 29 to 54% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5; ii) 35 to 68% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05, or 41 to 49% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9; iii) 0.01 to 10% by weight of a carboxy-reactive epoxy resin; iv) 0.01 to 10% by weight of polybutadiene rubber; v) 0 to 1% by weight of an injection solidification accelerator; The polybutylene terephthalate resin composition is characterized in that the total weight of the polybutylene terephthalate resins i) and ii) is 80 to 99% by weight.
[0025] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: The present invention provides a method for producing a polybutylene terephthalate resin composition, comprising the steps of feeding 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less, 0.01 to 10% by weight of a carboxy-reactive epoxy resin, 0.01 to 10% by weight of a polybutadiene rubber, and 0 to 1% by weight of an injection solidification accelerator into an extruder, and melt-kneading and extruding the mixture.
[0026] The injection solidification accelerator may contain an ethylene acrylate acid-based compound in an amount of 0.01 to 1% by weight relative to 100% by weight of the total amount of all components (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives) constituting the polybutylene terephthalate resin composition.
[0027] The present invention also provides a molded article produced by containing the polybutylene terephthalate resin composition described above.
[0028] The molded article may be an automobile part.
[0029] The automotive parts may be connectors, carburetor parts, fenders, spoilers, spark plug terminal plates, oil supply system parts, dashboards, automotive ignition, accelerator and clutch pedals. Effect of the Invention
[0030] The polybutylene terephthalate resin composition according to the present invention contains a polybutylene terephthalate resin having a specific intrinsic viscosity, a polybutadiene rubber and a carboxy-reactive epoxy resin, and can be molded into a molded article.
[0031] In addition, a molded article produced from the composition has excellent moldability and thus has an improved appearance quality, by simultaneously improving the solidification speed upon injection and impact strength, which are in a trade-off relationship, and by satisfying a balance of physical properties such as mechanical properties and fluidity.
[0032] Therefore, the polybutylene terephthalate resin composition according to the present invention can be applied in the field of molded products relating to fastening parts such as connectors which require the composition. [Brief description of the drawings]
[0033] [Figure 1] FIG. 2 is a schematic diagram illustrating a method for measuring lance cracks of a shot obtained according to an embodiment of the present invention. BEST MODE FOR CARRYING OUT THEINVENTION
[0034] In the following, the present invention will be described in more detail to facilitate understanding of the present invention.
[0035] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meaning, but should be interpreted in a meaning and concept that corresponds to the technical idea of the present invention, taking into consideration that the inventor can appropriately define the concept of the term in order to explain the invention in the best possible manner.
[0036] In this description, the meaning of "comprise" may be defined as "produced by polymerization comprising", "polymerized comprising", or "comprises as a unit derived from", unless otherwise defined.
[0037] Unless otherwise specified, all numbers, values and / or expressions expressing amounts of ingredients, reaction conditions, polymer compositions and formulations used in this description should be understood in all cases to be modified by the term "about" since such numbers are inherently approximations that reflect, among other things, various uncertainties of measurement that arise in obtaining such values. Also, when numerical ranges are disclosed in this description, such ranges are continuous and include all values from the minimum value to said maximum value, inclusive, unless otherwise specified. Furthermore, when such ranges refer to integers, they include all integers from the minimum value to said maximum value, inclusive, unless otherwise specified.
[0038] In this description, when a range is recited for a variable, the variable is understood to include all values within the recited range, including the recited endpoints of the range. For example, the range "5-10" is understood to include not only the values 5, 6, 7, 8, 9, and 10, but also any subranges such as 6-10, 7-10, 6-9, 7-9, etc., and any value between the integers that are valid within the recited range, such as 5.5-8.5, and 6.5-9, etc. Also, the range 10-30% is understood to include values such as 10%, 11%, 12%, 13%, etc., and all integers up to and including 30%, as well as any value between the integers that are valid within the recited range, such as 10.5%, 15.5%, 25.5%, etc.
[0039] The term "injection solidification accelerator" as used herein, unless otherwise specified, refers to a substance added during injection molding to shorten the solidification time. For reference, the solidification time may vary depending on the design and size of the mold of the injection machine even if the same material is used.
[0040] In this description, the melt index may be the melt index measured according to ISO 1133 at 250° C. under a load of 2.16 kg, unless otherwise specified.
[0041] The present inventors have confirmed that an automobile interior material manufactured using a polybutylene terephthalate resin composition containing a polybutylene terephthalate resin having a specific intrinsic viscosity, polybutadiene rubber, and a carboxy-reactive epoxy resin can simultaneously improve the injection solidification speed and impact strength, which are in a trade-off relationship, and can provide excellent product reliability and appearance quality by satisfying a balance of physical properties such as mechanical properties, fluidity, and heat resistance. Thus, the present inventors have completed a material for an automobile interior material as an unpainted product having excellent moldability and appearance quality while satisfying a balance of physical properties such as mechanical properties, fluidity, and heat resistance as in the present invention.
[0042] The polybutylene terephthalate resin composition according to one embodiment of the present invention includes 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less; 0.01 to 10% by weight of a carboxy-reactive epoxy resin; and 0.01 to 10% by weight of a polybutadiene rubber.
[0043] As another example, the polybutylene terephthalate resin composition may contain 1% by weight or less of an injection solidification accelerator.
[0044] The components constituting the polybutylene terephthalate resin composition will be specifically described below.
[0045] Base Resin The base resin according to one embodiment of the present invention is a polybutylene terephthalate resin, which imparts moldability to a polybutylene terephthalate resin composition containing the same and imparts chemical resistance to a molded article produced using the same.
[0046] The polybutylene terephthalate resin is a crystalline resin and has a crystallized structure that prevents the penetration of chemicals from the outside, and at the same time, improves the flowability of a polybutylene terephthalate resin composition containing the resin during injection molding, thereby providing excellent appearance quality.
[0047] The intrinsic viscosity (η) of the polybutylene terephthalate resin is characterized in that it includes both types having an intrinsic viscosity (η) of more than 1.05 and types having an intrinsic viscosity of 1.05 or less. In this case, the injection solidification speed and impact strength, which are in a trade-off relationship, can be improved at the same time.
[0048] As a specific example, the intrinsic viscosity (η) of the polybutylene terephthalate resin is characterized by simultaneously including one type having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5, and one type selected from a type having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05, and a type having an intrinsic viscosity (η) of less than 0.9. In this case, it is possible to appropriately provide a balance of physical properties between injection solidification speed and impact strength, which are in a trade-off relationship.
[0049] In this description, unless otherwise specified, the intrinsic viscosity is a value obtained by completely dissolving a sample to be measured in a methylene chloride solvent at a concentration of 0.05 g / ml, filtering the filtrate through a filter, and measuring the filtrate at 20° C. using an Ubbelohde viscometer.
[0050] The content of the polybutylene terephthalate resin may be, for example, 80 to 99% by weight, specifically 85 to 99% by weight, and preferably 90 to 99% by weight, based on the total amount of all components (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives) constituting the polybutylene terephthalate resin composition (100% by weight). If it is less than the above range, there is a drawback that the rigidity and heat resistance of a molded product manufactured using the polybutylene terephthalate resin composition containing the resin are reduced, and if it exceeds the above range, there is a drawback that cracks are generated in a molded product manufactured using the polybutylene terephthalate resin composition containing the resin.
[0051] The polybutylene terephthalate resin having an intrinsic viscosity (η) of less than 0.9 and the polybutylene terephthalate resin having an intrinsic viscosity of more than 0.9 and not more than 1.05 can be contained in a weight ratio of, for example, 30:70 to 60:40, specifically, 32:68 to 68:32, preferably 35:65 to 65:35. In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0052] The intrinsic viscosity (η) of the polybutylene terephthalate resin having a viscosity of more than 1.05 and not more than 1.5 may be, for example, 1.1 to 1.4, specifically 1.1 to 1.3, and preferably 1.1 to 1.2. In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0053] The intrinsic viscosity (η) of the polybutylene terephthalate resin having a viscosity of more than 0.9 and not more than 1.05 may be, for example, 0.91 to 1.05, specifically 0.95 to 1.05, and preferably 0.98 to 1.02. In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0054] The intrinsic viscosity (η) of the polybutylene terephthalate resin having an intrinsic viscosity of 0.7 or more and less than 0.9 may be, for example, 0.7 to 0.85, specifically 0.75 to 0.85, and preferably 0.8 to 0.85. In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0055] The polybutylene terephthalate resin having each of the above-mentioned intrinsic viscosities is not particularly limited, and may be prepared by a method known in the art or may be a commercially available material.
[0056] The polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5 may be contained in an amount of, for example, 29 to 55% by weight, specifically 30 to 55% by weight, and preferably 32 to 53% by weight, relative to 100% by weight of the total amount of all components constituting the polybutylene terephthalate resin composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives). In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0057] The polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05 can be contained in an amount of, for example, 0 to 68% by weight, specifically 40 to 68% by weight, preferably 35 to 68% by weight, more preferably 40 to 65% by weight, and even more preferably 40 to 60% by weight, relative to 100% by weight of the total amount of all components constituting the polybutylene terephthalate resin composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives). In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0058] The polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9 can be contained in an amount of, for example, 0 to 50% by weight, specifically 30 to 50% by weight, preferably 40 to 50% by weight, more preferably 40 to 48% by weight, and even more preferably 40 to 45% by weight, relative to 100% by weight of the total amount of all components constituting the polybutylene terephthalate resin composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives). In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0059] Carboxy reactive epoxy resin The term "carboxy-reactive epoxy resin" as used herein, unless otherwise specified, refers to an epoxy-functional alkylene (meth)acrylic copolymer formed from an epoxy-functional (meth)acrylic monomer and an alkylene.
[0060] As used herein, the term "(meth)acrylic" includes both acrylic and methacrylic monomers, and "(meth)acrylate" includes both acrylate and methacrylate monomers, unless otherwise specified.
[0061] Specific examples of the epoxy-functional (meth)acrylic monomers can include species containing 1,2-epoxy groups, such as glycidyl acrylate and glycidyl methacrylate.
[0062] The carboxy-reactive epoxy resin used in this description may be one or more selected from ethylene-n-butyl acrylate-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-acrylic acid ester-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer, ethylene-dimethacrylate-glycidyl methacrylate copolymer, ethylene-acrylate-glycidyl methacrylate copolymer, and ethylene-vinyl acetate-glycidyl methacrylate copolymer, as specific examples.
[0063] The carboxy-reactive epoxy resin described herein may be, for example, a copolymer containing 1-15% or 3-10% by weight of glycidyl methacrylate units, 60-74% or 63-74% by weight of ethylene units, and 20-30% or 25-30% by weight of n-butyl acrylate. If the content of the glycidyl methacrylate units is too high, the injection product produced using the polybutylene terephthalate resin composition containing the glycidyl methacrylate units may have a drawback in that the fluidity of the composition is reduced, impairing the appearance quality.
[0064] The content of the carboxy-reactive epoxy resin may be 0.01 to 10 wt%, preferably 0.1 to 4 wt%, more preferably 1 to 4 wt%, based on 100 wt% of all components constituting the composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber and additives). If the content of the carboxy-reactive epoxy resin is too high outside the above range, there is a problem of gas generation in the injection molded product on the surface of the molded product manufactured using the polybutylene terephthalate resin composition containing the same, which is disadvantageous in that the appearance quality is impaired.
[0065] Polybutadiene Rubber The polybutadiene rubber according to an embodiment of the present invention may be of a type that provides impact strength during injection molding of a molded article produced using the polybutylene terephthalate resin composition described herein.
[0066] In one embodiment of the present invention, the polybutadiene rubber may have an Izod impact strength (-30°C, 1 / 4'' thickness) of, for example, 10 kg / cm.cm or more, and an Izod impact strength (23°C, 1 / 4'' thickness) of, for example, 50 kg / cm.cm or more, measured in accordance with ASTM D256. In this case, the polybutadiene rubber may have a good balance of physical properties such as mechanical properties, fluidity, and heat resistance.
[0067] As a specific example, the polybutadiene rubber may have an Izod impact strength (-30°C, 1 / 4" thickness) measured in accordance with ASTM D256 of, for example, 10 to 100 kg / cm.cm, and at the same time, an Izod impact strength (23°C, 1 / 4" thickness) of, for example, 50 to 150 kg / cm.cm. In this case, a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied.
[0068] The weight ratio of linear type and branched type polybutadiene contained in the polybutadiene rubber may be adjusted to 25:75 to 90:10.
[0069] The linear and branched polybutadiene may be premixed in a liquid phase at a weight ratio of 50:75 to 50:25, and then solidified.
[0070] The linear type polybutadiene is obtained by polymerizing 1,3-butadiene or a butadiene derivative using a transition metal Ziegler-Natta catalyst in the presence of a non-polar solvent, and may be obtained by including a nickel catalyst composed of a nickel salt, an organoaluminum, and a fluoride compound as the transition metal Ziegler-Natta catalyst, and a dialkylzinc compound represented by the following Chemical Formula 1 as a molecular weight regulator.
[0071] Chemical formula 1: R1-Zn-R2 (In the above formula, R1 and R2 are the same or different alkyl groups having 1 to 5 carbon atoms.)
[0072] The branched type polybutadiene may be obtained by polymerizing 1,3-butadiene or a butadiene derivative using a transition metal Ziegler-Natta catalyst in the presence of a non-polar solvent, and the transition metal Ziegler-Natta catalyst may be a nickel catalyst composed of a nickel salt, a fluoride compound, an organoaluminum, and an aluminoxane, and the reactivity of the organoaluminum and the aluminoxane may be adjusted.
[0073] The nickel salt may be a carboxylate having a saturated, unsaturated, cyclic or linear structure having 8 to 20 carbon atoms, and specific examples of the carboxylate include nickel octoate, nickel versatate, and nickel naphthenate.
[0074] The 1,3-butadiene or butadiene derivative may be at least one selected from 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, myrcene, and derivatives thereof.
[0075] The non-polar solvent may be one or more selected from pentane, hexane, isopentane, heptane, octane, isooctane, cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, ethylcyclohexane, benzene, toluene, ethylbenzene, and xylene.
[0076] In one embodiment of the present invention, the polybutadiene rubber may have a #20 mesh passing portion of 100% of the total number of all particles, for example 3% or less, specifically 0.01 to 3%, and preferably 0.1 to 3%, in which case a balance of physical properties such as mechanical properties, flowability, and heat resistance can be satisfied.
[0077] The polybutadiene rubber of the present invention may be, for example, 0.01 to 10% by weight, preferably 0.1 to 5% by weight, more preferably 0.1 to 5% by weight, even more preferably 1 to 5% by weight, and most preferably 2 to 5% by weight, based on the total of 100% by weight of all components constituting the composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives). In this case, the drawback of slowing down the solidification speed in exchange for imparting appropriate impact resistance to a molded article produced using a polybutylene terephthalate resin composition containing the composition can be overcome.
[0078] The butadiene resin is not particularly limited, and may be prepared by a method known in the art or may be a commercially available material, such as EM538 from LG Chem.
[0079] Injection solidification accelerator According to an embodiment of the present invention, the injection solidification accelerator may be included to shorten the solidification speed during injection molding of a molded product manufactured using the polybutylene terephthalate resin composition and improve the crystallinity thereof to provide product reliability.
[0080] The injection solidification accelerator may be, for example, an inorganic injection solidification accelerator such as talc, wollastonite, or mica, or an organic injection solidification accelerator such as an ethylene acrylate acid-based compound. Among these, when an organic injection solidification accelerator is used together with the polybutadiene rubber, it can realize a fast solidification speed characteristic and maintain high impact strength due to low impact drop, thereby reducing the occurrence of cracks in parts and being easily applicable to small / thin film materials.
[0081] The ethylene acrylate acid-based compound may, for example, include an ethylene compound and an unsaturated acrylate type.
[0082] In one embodiment of the present invention, the ethylene acrylate acid-based compound may have a bulk density of 0.25 g / cc or more as measured in accordance with ASTM D1895, and in this case, the balance of physical properties such as mechanical properties, fluidity, and heat resistance may be satisfied.
[0083] The ethylene acrylate acid-based compound described herein may be, for example, a copolymer containing 1-15% or 3-10% by weight of ethylene units, 60-74% or 63-74% by weight of acrylate units, and 20-30% or 25-30% by weight of acrylic acid units. If the content of ethylene units is too high, the injection product produced using the polybutylene terephthalate resin composition containing the same may have a drawback in that the fluidity of the composition is reduced, impairing the appearance quality.
[0084] The content of the ethylene acrylate acid-based compound may be, for example, 0.01 to 1 wt%, preferably 0.01 to 0.8 wt%, and more preferably 0.1 to 0.5 wt%, based on 100 wt% of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If the content of the ethylene acrylate acid-based compound is too high outside the above range, there is a drawback in that cracks are generated on the surface of a molded product manufactured using a polybutylene terephthalate resin composition containing the same.
[0085] The injection solidification accelerator is not particularly limited, and may be prepared by a method known in the art or may be a commercially available material, such as Dupont's PTW series.
[0086] Additives The polybutylene terephthalate resin composition according to an embodiment of the present invention may contain a suitable additive to improve its flowability.
[0087] The additives may be, for example, 0.01 to 10% by weight, preferably 0.1 to 8% by weight, more preferably 0.1 to 5% by weight, even more preferably 1 to 5% by weight, and most preferably 1 to 3% by weight, based on 100% by weight of all components constituting the composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives).
[0088] The polybutylene terephthalate resin composition according to an embodiment of the present invention may contain a suitable additive to improve its flowability.
[0089] The additive may be, for example, 0.01 to 10% by weight, preferably 0.1 to 8% by weight, more preferably 0.1 to 5% by weight, even more preferably 1 to 5% by weight, and most preferably 1 to 3% by weight, based on the total of 100% by weight of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If it is less than the above range, there is a drawback that the solidification speed is slowed down and cracks are generated in a molded article manufactured using a polybutylene terephthalate resin composition containing this, and if it exceeds the above range, there is a drawback that the rigidity and heat resistance properties of a molded article manufactured using a polybutylene terephthalate resin composition containing this are reduced.
[0090] The additives may include, for example, one or more selected from a lubricant, an antioxidant, and a colorant.
[0091] The lubricant is not particularly limited as long as it can ensure the ease of removal and flowability of an injection screw used to produce a molded article from a polybutylene terephthalate resin composition containing the lubricant.
[0092] The lubricant is not particularly limited as long as it can be used in the present invention and can ensure the above-mentioned properties, but preferably contains a polyethylene wax.
[0093] The lubricant may be, for example, 0.01 to 10% by weight, preferably 0.1 to 3% by weight, more preferably 0.1 to 2% by weight, even more preferably 0.1 to 1% by weight, and most preferably 0.1 to 0.5% by weight, based on 100% by weight of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If the content of the lubricant is too high outside the above range, there is a disadvantage that the surface of a molded product produced using the polybutylene terephthalate resin composition containing the lubricant may have appearance problems such as unevenness, which impairs the appearance quality.
[0094] The lubricant may be any of various known types as long as it does not adversely affect the polybutylene terephthalate resin composition of the present invention. Among commercially available materials, a polyethylene compound having the product name LC102N may be representatively used.
[0095] The antioxidant is not particularly limited as long as it can prevent denaturation of a molded article produced using a polybutylene terephthalate resin composition containing the antioxidant due to high temperatures.
[0096] The antioxidant is not particularly limited as long as it can ensure the above properties. For example, the antioxidant may include a primary antioxidant, a secondary antioxidant, or both of them. In this case, it has the effect of preventing oxidation due to heat during the extrusion process and having excellent mechanical properties.
[0097] The primary antioxidant and the secondary antioxidant may be included in a weight ratio of 1:0.5 to 1.5, preferably 1:0.7 to 1.2, which has the effect of providing a balance between processability and physical properties.
[0098] The primary antioxidant may be a phenol-based antioxidant, and may include, for example, a hindered phenol-based stabilizer having a crystallization temperature (Tm) of 110 to 130°C. Specific examples include tetrakis[ethylene-3-(3,5-di-t-butyl-hydroxyphenyl)propionate], octadecyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, or a combination thereof.
[0099] The phenol-based antioxidant may be, for example, 0.01 to 10% by weight, preferably 0.01 to 3% by weight, more preferably 0.01 to 2% by weight, even more preferably 0.01 to 1% by weight, and most preferably 0.05 to 0.5% by weight, based on 100% by weight of all components constituting the composition (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives). If the content of the phenol-based antioxidant is too high, there is a drawback in that the surface of a molded product produced using the polybutylene terephthalate resin composition containing the phenol-based antioxidant may have appearance problems such as unevenness, which impairs the appearance quality.
[0100] The secondary antioxidant may be a phosphorus-based antioxidant, and an example thereof may include a phosphite-based antioxidant, and specific examples thereof may include tris-(2,4-di-tert-butylphenyl)phosphite, di-(2,4-di-t-butylphenyl)pentaerythritol diphosphite, or a combination thereof.
[0101] The phosphorus-based antioxidant may be, for example, 0.01 to 10% by weight, preferably 0.01 to 3% by weight, more preferably 0.01 to 2% by weight, even more preferably 0.01 to 1% by weight, and most preferably 0.1 to 0.5% by weight, based on 100% by weight of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If the content of the phosphorus-based antioxidant is too high, there is a drawback in that the surface of a molded product produced using the polybutylene terephthalate resin composition containing the phosphorus-based antioxidant may have appearance problems such as unevenness, which impairs the appearance quality.
[0102] The antioxidant may be any of various known types as long as it does not adversely affect the polybutylene terephthalate resin composition of the present invention. Representative examples of commercially available antioxidants include a bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite compound with the product name Songnox 6260 as a secondary antioxidant and a pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) compound with the product name IR1010 as a primary antioxidant, but are not limited thereto.
[0103] The colorants of the present invention may be colorants including pigments or dyes.
[0104] The pigment may be, for example, an inorganic pigment.
[0105] The inorganic pigment may be at least one selected from the group consisting of metal compounds such as Ti, Pb, Fe, and Cr, and carbon black, and the metal compound is preferably a metal oxide or metal hydroxide. Specific examples of the inorganic pigment include white inorganic pigments such as TiO2 and zinc oxide; black inorganic pigments such as carbon black and graphite; red inorganic pigments such as IOR, cadmium red, and red lead (Pb3O4); yellow inorganic pigments such as chrome yellow, zinc chromate, and cadmium yellow; and green inorganic pigments such as chrome green and zinc green. The most preferred inorganic pigment is carbon black, which is a black inorganic pigment.
[0106] The colorant may be, for example, 0.01 to 10 parts by weight, preferably 0.01 to 3 parts by weight, more preferably 0.1 to 3 parts by weight, and even more preferably 0.5 to 3 parts by weight, based on 100 parts by weight of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If the content of the colorant is too high, there is a drawback in that the crack quality of a molded product produced using the polybutylene terephthalate resin composition containing the colorant is impaired.
[0107] Optionally, a hydrolysis inhibitor may further be included.
[0108] The hydrolysis inhibitor may be any of various known types as long as it does not adversely affect the polybutylene terephthalate resin composition of the present invention. Among commercially available substances, a representative example is an organic phosphate compound such as sodium monophosphate having the chemical formula NaH2PO4.
[0109] The hydrolysis inhibitor may be, for example, 0.01 to 5 wt%, preferably 0.1 to 3 wt%, more preferably 0.1 to 2 wt%, even more preferably 0.1 to 1 wt%, and most preferably 0.1 to 0.5 wt%, based on 100 wt% of all components constituting the composition (base resin, carboxy reactive epoxy resin, polybutadiene rubber, and additives). If the content of the hydrolysis inhibitor is too high outside the above range, there is a disadvantage that the appearance problem such as unevenness occurs on the surface of a molded product manufactured using a polybutylene terephthalate resin composition containing the hydrolysis inhibitor, which impairs the appearance quality.
[0110] Polybutylene terephthalate resin composition The polybutylene terephthalate resin composition according to one embodiment of the present invention is characterized by including 80-99 wt % of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less, 0.01-10 wt % of a carboxy-reactive epoxy resin, 0.01-10 wt % of a polybutadiene rubber, and 0-1 wt % of an injection solidification accelerator. In this case, the injection solidification speed and impact strength can be improved at the same time, and a balance of physical properties such as mechanical properties, fluidity, and heat resistance can be satisfied, thereby providing excellent product reliability and appearance quality.
[0111] The polybutylene terephthalate resin composition according to another embodiment of the present invention is characterized by comprising 29-55 wt% of polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5, 0-68 wt% of polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05, 0-50 wt% of polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9, 0.01-10 wt% of a carboxy-reactive epoxy resin, 0.01-10 wt% of a polybutadiene rubber, and 0-1 wt% of an injection solidification accelerator. In this case, the injection solidification speed and impact strength are improved at the same time, and the balance of physical properties such as mechanical properties, fluidity, and heat resistance is satisfied, and excellent product reliability and appearance quality can be provided, making it suitable for application as a molded product.
[0112] The polybutylene terephthalate resin composition according to yet another embodiment of the present invention comprises i) 29 to 54% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5, ii) 35 to 68% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05, or 41 to 49% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9, and iii) 0. 0.01-10% by weight of polybutadiene rubber, iv) 0.01-10% by weight of polybutadiene rubber, and v) 0-1% by weight of an injection solidification accelerator, the total weight of the polybutylene terephthalate resins i) and ii) being 80-99% by weight. In this case, the injection solidification speed and impact strength are improved simultaneously, and a balance of physical properties such as mechanical properties, fluidity, and heat resistance is satisfied, and excellent product reliability and appearance quality can be provided, making it suitable for use as a molded product.
[0113] The polybutylene terephthalate resin composition of the present invention may have a flow index (250° C., 2.16 kgf) measured in accordance with ISO 1133 of, for example, 10 g / 10 min or more, specifically, 10 to 30 g / 10 min.
[0114] The polybutylene terephthalate resin composition of the present invention may have a tensile strength measured in accordance with ISO 527 of, for example, 45 MPa or more, specifically, 45 to 50 MPa.
[0115] The polybutylene terephthalate resin composition of the present invention may have a tensile elongation measured in accordance with ISO 527 of, for example, 15% or more, specifically, 20 to 85%.
[0116] The polybutylene terephthalate resin composition of the present invention has an Izod impact strength (23°C, notched) measured in accordance with ISO 180 of, for example, 7 kJ / m 2 , for example, 7.8 to 10 kJ / m 2 may be also possible.
[0117] The polybutylene terephthalate resin composition of the present invention may have a heat distortion temperature measured under a load of 0.45 MPa in accordance with ISO 75 of, for example, 100°C or higher, specifically, 100 to 130°C.
[0118] The polybutylene terephthalate resin composition of the present invention may have a heat distortion temperature measured under a high load of 1.8 MPa in accordance with ISO 75 of, for example, 40°C or higher, specifically, 45 to 55°C.
[0119] The polybutylene terephthalate resin composition of the present invention may have a flexural modulus measured in accordance with ISO 178 of, for example, 1700 MPa or more, specifically, 1750 to 2100 MPa.
[0120] The polybutylene terephthalate resin composition of the present invention may have a flexural strength measured in accordance with ISO 178 of, for example, 60 MPa or more, specifically, 64 to 80 MPa.
[0121] Method for producing polybutylene terephthalate resin composition The method for producing the polybutylene terephthalate resin composition of the present invention will be described below. In the description of the method for producing the polybutylene terephthalate resin composition of the present invention, all of the contents of the polybutylene terephthalate resin composition described above are included.
[0122] As an example, a method for producing a polybutylene terephthalate resin composition described herein includes the steps of feeding 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less, 0.01 to 10% by weight of a carboxy-reactive epoxy resin, 0.01 to 10% by weight of a polybutadiene rubber, and 0 to 1% by weight of an injection solidification accelerator into an extruder, and melt-kneading and extruding the mixture.
[0123] The injection solidification accelerator may contain an ethylene acrylate acid-based compound in an amount within the range of 0.01 to 1% by weight relative to 100% by weight of the total amount of all components (base resin, carboxy-reactive epoxy resin, polybutadiene rubber, and additives) constituting the polybutylene terephthalate resin composition.
[0124] The melt-kneading step may include, for example, other additives as described above.
[0125] The melt-kneading and extruding steps may be performed using at least one selected from the group consisting of a single screw extruder, a twin screw extruder, and a Banbury mixer, and preferably a twin screw extruder. The composition is uniformly mixed using the extruder and then extruded to obtain, for example, a pellet-shaped polybutylene terephthalate resin composition, which has the effect of being excellent in mechanical properties, thermal properties, plating adhesion, and appearance quality.
[0126] The step of producing pellets using the extrusion kneader can be performed, for example, at an extrusion temperature of 250 to 300° C., a feed rate (Flow ratio, F / R) of 50 to 90 kg / hr, and a screw rotation speed of 200 to 490 rpm, and preferably at an extrusion temperature of 250 to 270° C., an F / R of 50 to 90 kg / hr, and a screw rotation speed of 250 to 350 rpm.
[0127] After extruding the polybutylene terephthalate resin composition, the step of injecting the composition at an injection temperature of 240 to 280°C, specifically 250 to 270°C, a mold temperature of 40 to 80°C, specifically 50 to 70°C, and at an injection speed of 10 to 50 mm / sec, specifically 20 to 40 mm / sec may be included.
[0128] Further, a molded article containing the polybutylene terephthalate resin composition of the present invention will be described. In describing a molded article containing the polybutylene terephthalate resin composition of the present invention, all of the contents of the polybutylene terephthalate resin composition described above are included.
[0129] molded product The polybutylene terephthalate resin composition of the present invention can be effectively used for molded products requiring moldability, mechanical properties, high load heat resistance and fast injection solidification speed through sufficient complementation between components.
[0130] The molded product can be manufactured by a method commonly used in the art. For example, the molded product can be manufactured by a molding method such as injection molding, injection compression molding, extrusion molding (sheet casting), press molding, pressure molding, hot bending molding, compression molding, calendar molding, or rotational molding using the melt-kneaded product, pellets, or sheet (plate) molded from the polybutylene terephthalate resin composition according to the present invention as a raw material.
[0131] As an example, the polybutylene terephthalate resin composition described herein can be produced into pellets by using a twin-screw extruder (φ40, L / D:42, equipped with SM Platek) set at 250°C and feeding a base (polybutylene terephthalate) resin, a carboxy-reactive epoxy resin, a polybutadiene rubber, an injection solidification accelerator, and additives into the main inlet at a feed rate of 50 kg / h at 250 rpm, and melt-kneading and extruding.
[0132] As another example, the polybutylene terephthalate resin composition described herein can be produced into pellets by melt-kneading and extruding a twin-screw extruder (φ40, L / D:42, equipped with SM Platek) set at 280°C at 375 rpm, feeding a base (polybutylene terephthalate) resin and a carboxy-reactive epoxy resin into the main inlet, and feeding polybutadiene rubber, an injection solidification accelerator and additives into the auxiliary inlet at a feed rate of 75 kg / h.
[0133] As yet another example, the polybutylene terephthalate resin composition described herein can be melt-kneaded and extruded to produce pellets using a twin-screw extruder (φ40, L / D:42, equipped with SM Platek) set at 250°C at 250 rpm, by feeding a base (polybutylene terephthalate) resin, a carboxy-reactive epoxy resin, and a polybutadiene rubber into the main inlet and feeding an injection solidification accelerator and additives into the auxiliary inlet at a feed rate of 50 kg / h.
[0134] The pellets can be fed into an injection molding machine to produce a molded article.
[0135] In order to indirectly confirm the physical properties of the produced molded product, the pellets are injected into an injection molding machine (ENGEL, 80 tons) at an injection temperature of 260°C, a mold temperature of 60°C, and an injection speed of 30 mm / sec to produce ISO standard test pieces.
[0136] Based on the measurement results of the produced test pieces, the polybutylene terephthalate resin composition of the present invention may have a flow index (250°C, 2.16 kgf) measured in accordance with ISO 1133 of, for example, 10 g / 10 min or more, specifically, 10 to 30 g / 10 min.
[0137] The polybutylene terephthalate resin composition of the present invention may have a tensile strength measured in accordance with ISO 527 of, for example, 45 MPa or more, specifically, 45 to 50 MPa.
[0138] The polybutylene terephthalate resin composition of the present invention may have a tensile elongation measured in accordance with ISO 527 of, for example, 15% or more, specifically, 20 to 85%.
[0139] The polybutylene terephthalate resin composition of the present invention has an Izod impact strength (23°C, notched) measured in accordance with ISO 180 of, for example, 7 kJ / m 2 , for example, 7.8 to 10 kJ / m 2 may be also possible.
[0140] The polybutylene terephthalate resin composition of the present invention may have a heat distortion temperature measured under a load of 0.45 MPa in accordance with ISO 75 of, for example, 100°C or higher, specifically, 100 to 130°C.
[0141] The polybutylene terephthalate resin composition of the present invention may have a heat distortion temperature measured under a high load of 1.8 MPa in accordance with ISO 75 of, for example, 40°C or higher, specifically, 45 to 55°C.
[0142] The polybutylene terephthalate resin composition of the present invention may have a flexural modulus measured in accordance with ISO 178 of, for example, 1700 MPa or more, specifically, 1750 to 2100 MPa.
[0143] The polybutylene terephthalate resin composition of the present invention may have a flexural strength measured in accordance with ISO 178 of, for example, 60 MPa or more, specifically, 64 to 70 MPa.
[0144] The solidification speed (injection cooling time) of the polybutylene terephthalate resin composition of the present invention, measured in accordance with an internal evaluation method, can be reduced to, for example, 14 seconds or less, specifically, 6 to 14 seconds, and preferably about 6 to 12 seconds.
[0145] The polybutylene terephthalate resin composition of the present invention has a maximum peak pressure of, for example, 1000 kgf / cm 2 The above is a specific example of 1000-1150kgf / cm 2 may be also possible.
[0146] The polybutylene terephthalate resin composition of the present invention may be undamaged when an iron rod is inserted into a lance inside a fastening part and the lance is pushed up strongly using the principle of leverage to check for damage.
[0147] The molded article may specifically be a fastening part of a vehicle, but is not limited to a particular type.
[0148] That is, the polybutylene terephthalate resin composition according to one embodiment of the present invention is characterized by including a polybutylene terephthalate resin having a specific intrinsic viscosity, a polybutadiene rubber, and a carboxy-reactive epoxy resin. The molded product manufactured from the composition has the advantage of simultaneously improving the injection solidification speed and impact strength, which are in a trade-off relationship due to the change in the materials used from conventional materials, and satisfying the balance of physical properties such as mechanical properties, fluidity, and heat resistance, thereby providing excellent product reliability and appearance quality.
[0149] In describing the polybutylene terephthalate resin composition of the present invention, its production method, and molded products, other conditions, equipment, etc. that are not explicitly described can be appropriately selected within the range commonly used in the art, and it is clearly stated that there are no particular limitations.
[0150] The present invention may, however, be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein.
[0151] [Example] Example 1 and Comparative Examples 1 to 5 (Experiments not including injection solidification accelerator) The raw materials used in the examples and comparative examples are as follows. A-1) Polybutylene terephthalate resin: Intrinsic viscosity (IV) 0.83, product name TH6082A A-2) Polybutylene terephthalate resin: IV, 1.0 Product name TH6098A A-3) Polybutylene terephthalate resin: IV1.12, product name PBT1100-211S (B) Carboxy-reactive epoxy resin: Ethylene / n-butyl acrylate / glycidyl methacrylate resin, Dupont product name PTW (C) Polybutadiene rubber C-1) Polybutadiene rubber, LG Chem's product name EM538 C-2) Polybutadiene rubber, LG Chem's product name EM500 (D) Injection solidification accelerator D-1) Ethylene acrylate acid compound: Bruggemann product name P250 D-2) Inorganic injection solidification accelerator: Koch product name KCM6300 (Additives) (E) Lubricant: LC102N (F) Antioxidants F-1) Primary antioxidant: IR1010 F-2) Secondary antioxidant: Songnox 6260 (G) Colorant: LG Chemical, product name NR9089 Black (H) Polyethylene elastomer, LG Chem, product name 1055D
[0152] The raw materials of the polybutylene terephthalate resin composition shown in Table 1 below were mixed and extruded to produce a polybutylene terephthalate resin composition having a uniform dispersion degree in the form of pellets. The pellets were then heated and injected into a mold, and cooled to produce parts. Through an injection process, a test piece that can be used as a molded product was prepared.
[0153] Specifically, the components shown in Table 1 below are mixed in a mixer, and then fed into a main inlet at a feed rate of 75 kg / h at 250 rpm using a twin-screw extruder (φ40, L / D: 42, equipped with SM Platek) set at 250°C, and extruded to produce polybutylene terephthalate resin composition pellets.
[0154] The produced pellets were dried in a convection oven at 80°C for at least 4 hours, and then injected into an injection molding machine (ENGEL, 80 ton) at an injection temperature of 260°C, a mold temperature of 60°C, and an injection speed of 30 mm / sec to prepare ISO test specimens.
[0155] [Table 1]
[0156] (The raw materials used in Table 1 above, A-1 to F-2, are all combined to 100 parts by weight, and the G component is added in parts by weight units.)
[0157] Test Example 1: Evaluation of the physical properties of molded test pieces The physical properties of the molded test pieces produced in Example 1 and Comparative Examples 1 to 5 were evaluated. The evaluation criteria were as follows. -Melt Index: According to ISO 1133 (250°C, 2.16 kg) - Tensile strength and elongation: according to ISO 527 (50mm / min) -Impact strength (IZOD): according to ISO 180 / 1A (Notched, 23°C) - Heat distortion temperature: According to ISO 75, high load of 1.82 MPa and low load of 0.45 MPa are used. -Flexural strength, flexural modulus: According to ISO 178 (4mm, SPAN64, speed 2mm / min) -Solidification speed (injection cooling time): The cooling time required until the material solidifies and no longer changes length was measured in seconds. - Maximum peak pressure of injection: The maximum peak pressure applied to the injection machine at the time of solidification in kgf / cm 2 Measured in units. - Parts lance crack: Parts lance crack was measured using the method shown in Figure 1. Figure 1 below is a schematic diagram of the part lance crack measurement method. An iron rod was inserted into the lance part inside the connector test piece on the left side of Figure 1, and the lance was pushed hard using the principle of leverage to bounce up, and the presence or absence of damage was visually observed (see the right side of Figure 1). If damage occurred, it was marked as NG, and if no damage occurred, it was marked as OK.
[0158] The results measured according to the above evaluation criteria are shown in Table 2 below.
[0159] [Table 2]
[0160] Referring to Tables 1 and 2, the polybutylene terephthalate resin composition of Example 1 according to the present invention has high impact strength, flexural modulus, high-load heat distortion temperature, and flow index, and the solidification speed and maximum peak pressure of injection are shortened, and no part lance crack occurs. Therefore, it can be confirmed that a molded product manufactured using the composition basically satisfies physical properties such as impact strength, tensile strength, and flexural strength, while having excellent processability and high-load heat resistance, and the occurrence of appearance defects is reduced due to the shortened solidification speed, thereby providing both product reliability and appearance quality.
[0161] On the other hand, in Comparative Examples 1 to 5, in which the ratio of intrinsic viscosities was not within the appropriate range, it was confirmed that the fluidity was reduced and the solidification speed was gradually slower than in Example 1.
[0162] In particular, in Comparative Example 3, in which polybutylene terephthalate resin was used alone without adjusting the intrinsic viscosity ratio, the flowability was reduced due to high viscosity, resulting in reduced injection moldability, and problems such as non-molding occurred in small / thin molds. In Comparative Example 4, poor results were observed, with parts cracking due to reduced impact strength.
[0163] Moreover, it was confirmed that Comparative Example 5, which used a polybutadiene rubber with an unsuitable composition, gave poor results in terms of reduced rigidity and impact strength.
[0164] Furthermore, it was confirmed that when an inorganic injection solidification accelerator was used, the impact strength decreased, causing cracks in the parts.
[0165] Examples 2 to 4 and Comparative Examples 6 to 14 The raw materials of the polybutylene terephthalate resin composition shown in Tables 3 and 4 below were mixed, and then extruded to produce a polybutylene terephthalate resin composition having a uniform dispersion degree in the form of pellets. The pellets were then heated and injected into a mold, and cooled to produce a part. Through an injection process, a test piece that can be used as a molded product was prepared. Unless otherwise specified, the extrusion and injection conditions used in Example 1 were applied in the same manner.
[0166] [Table 3]
[0167] [Table 4]
[0168] (For reference, the total weight percent of the raw materials A-1 to H used in Tables 3 and 4 is 100 weight percent.)
[0169] Test Example 2: Evaluation of the physical properties of molded test pieces The physical properties of the molded test pieces produced in Examples 2 to 4 and Comparative Examples 6 to 14 were evaluated, and the measurement results are shown in Tables 5 and 6 below.
[0170] [Table 5]
[0171] [Table 6]
[0172] Referring to Tables 3 to 6, the polybutylene terephthalate resin compositions of Examples 2 to 4 according to the present invention have high impact strength, flexural modulus, high-load heat distortion temperature, and flow index, and the solidification speed and maximum peak pressure of injection are shortened, and no part lance crack occurs. Therefore, it can be confirmed that molded products manufactured using the compositions basically satisfy physical properties such as impact strength, tensile strength, and flexural strength, while having excellent processability and high-load heat resistance, and the occurrence of appearance defects is reduced due to the shortened solidification speed, thereby providing both product reliability and appearance quality.
[0173] On the other hand, in Comparative Examples 6 to 14, in which the ratio of intrinsic viscosity was not within the appropriate range, the fluidity was reduced, the solidification speed gradually slowed, and the impact strength was significantly reduced compared to Examples 2 to 4.
[0174] That is, the polybutylene terephthalate resin composition according to one embodiment of the present invention includes a composite resin including a specific weight % of polybutylene terephthalate resin and a polyethylene terephthalate resin, a specific weight % of a (meth)acrylate compound-conjugated diene compound-aromatic vinyl compound copolymer, a hydrolysis stabilizer mixed with a carboxy-reactive epoxy resin, and an injection solidification accelerator. As a result, a molded product manufactured from the composition simultaneously improves the injection solidification speed and impact strength, which are in a trade-off relationship, and satisfies a balance of physical properties such as mechanical properties, fluidity, and heat resistance, thereby providing excellent product reliability and appearance quality.
Claims
1. 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less; 0.01 to 10% by weight of a carboxy-reactive epoxy resin; and 0.01 to 10% by weight of polybutadiene rubber.
2. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less contains a polybutylene terephthalate resin having an intrinsic viscosity of less than 0.9 and a polybutylene terephthalate resin having an intrinsic viscosity of more than 0.9 and 1.05 or less in a weight ratio of 30:70 to 60:
40.
3. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 contains 29 to 55% by weight of the polybutylene terephthalate resin having an intrinsic viscosity of more than 1.05 and not more than 1.5, relative to a total of 100% by weight of the base resin, the carboxy-reactive epoxy resin, the polybutadiene rubber, the additives, and any injection solidification accelerator constituting the polybutylene terephthalate resin composition.
4. 2. The polybutylene terephthalate resin composition of claim 1, wherein the carboxy-reactive epoxy resin comprises one or more selected from ethylene-n-butyl acrylate-glycidyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-acrylic acid ester-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer, ethylene-dimethacrylate-glycidyl methacrylate copolymer, ethylene-acrylate-glycidyl methacrylate copolymer, and ethylene-vinyl acetate-glycidyl methacrylate copolymer.
5. The polybutylene terephthalate resin composition according to claim 1, wherein the carboxy-reactive epoxy resin contains 1 to 15 weight percent of units derived from glycidyl methacrylate.
6. The polybutadiene rubber has a bulk density measured in accordance with ASTM D1895 of 0.25 g / cc or more, an Izod impact strength (-30°C, 1 / 4" thickness) measured in accordance with ASTM D256 of 10 kg / cm.cm or more, and an Izod impact strength (23°C, 1 / 4" thickness) of 50 kg / cm.cm or more, and a #20 mesh passing portion of all particles is 3% or less of the total number of all particles (100%).
7. The polybutylene terephthalate resin composition according to claim 1, further comprising at least one injection solidification accelerator selected from the group consisting of talc, wollastonite and ethylene acrylate acid compounds in an amount of 1% by weight or less.
8. The polybutylene terephthalate resin composition according to claim 7, wherein the ethylene acrylate acid-based compound is contained in an amount of 0.01 to 1% by weight relative to a total of 100% by weight of the base resin, the carboxy-reactive epoxy resin, the polybutadiene rubber, the additives, and the injection solidification accelerator constituting the polybutylene terephthalate resin composition.
9. 10. The polybutylene terephthalate resin composition of claim 1, further comprising an additive selected from a lubricant, an antioxidant, and a colorant.
10. 29 to 55% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5; 0 to 68% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05; 0 to 50% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9; 0.01 to 10% by weight of a carboxy-reactive epoxy resin; 0.01 to 10% by weight of polybutadiene rubber; and 0 to 1 weight percent of an injection solidification accelerator.
11. i) 29 to 54% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and not more than 1.5; ii) 35 to 68% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 0.9 and not more than 1.05, or 41 to 49% by weight of a polybutylene terephthalate resin having an intrinsic viscosity (η) of 0.7 or more and less than 0.9; iii) 0.01 to 10 wt. % of a carboxy-reactive epoxy resin; iv) 0.01 to 10% by weight of polybutadiene rubber; v) 0 to 1 wt. % of an injection solidification accelerator; A polybutylene terephthalate resin composition, wherein the total weight of the polybutylene terephthalate resins i) and ii) is 80 to 99% by weight.
12. A method for producing a polybutylene terephthalate resin composition, comprising the steps of melt-kneading and extruding, using an extruder, 80 to 99% by weight of a base resin including a polybutylene terephthalate resin having an intrinsic viscosity (η) of more than 1.05 and a polybutylene terephthalate resin having an intrinsic viscosity (η) of 1.05 or less, 0.01 to 10% by weight of a carboxy-reactive epoxy resin, 0.01 to 10% by weight of a polybutadiene rubber, and 0 to 1% by weight of an injection solidification accelerator.
13. A molded article comprising the polybutylene terephthalate resin composition according to any one of claims 1 to 11.
14. The molded article according to claim 13, which is a fastening part for automotive electrical equipment.
Citation Information
Patent Citations
Flame-retarding polyester composition
JP1991020351A
Polybutylene terephthalate resin composition
JP1994049337A
Polybutylene terephthalate resin composition and resin-molded article using the same
JP2012201857A
High frequency signal transmission component and high frequency electric / electronic apparatus
JP2013131576A
Vibration welding polybutylene terephthalate composition
JP2014125589A