Nonaqueous electrolyte composition and lithium secondary battery containing same
The non-aqueous electrolyte composition with a high oxidation potential window and protective film-forming additives addresses the issue of side reactions at both electrodes, enhancing stability and safety in lithium secondary batteries.
Patent Information
- Application Number
- JP2024531135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-06-28
AI Technical Summary
Conventional electrolytes in lithium secondary batteries fail to suppress side reactions at both the positive and negative electrodes, especially under high voltage conditions, leading to decomposition and gas generation, which limits their performance and safety.
A non-aqueous electrolyte composition with an oxidation potential window of 4.5V or more, containing specific electrolyte additives that form a protective film on both positive and negative electrodes, enhancing oxidation stability and suppressing side reactions.
The electrolyte composition improves oxidation stability, preventing decomposition and gas generation, thereby extending battery life and reducing the risk of explosion, while maintaining high voltage performance.
Smart Images

Figure 2024542550000001 
Figure 2024542550000002 
Figure 2024542550000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonaqueous electrolyte composition, and more particularly to a nonaqueous liquid electrolyte composition that enables the production of a battery having an improved oxidation potential window, excellent oxidation stability, and high energy density, and a lithium secondary battery containing the same.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0107593 dated August 26, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]
[0003] 2. Description of the Related Art In recent years, secondary batteries have been widely used not only in small devices such as portable electronic devices, but also in medium- to large-sized devices such as battery packs for hybrid and electric vehicles and power storage devices.
[0004] Such secondary batteries are manufactured by applying a composition containing an electrode active material to a current collector in a suitable thickness and length, and drying the composition, or forming the electrode active material itself into a film to form a positive electrode and a negative electrode, and then winding or stacking these together with a separator, which is an insulator, to form an electrode assembly, which is then placed in a can or a similar container and filled with an electrolyte.
[0005] Here, if the potential window of the electrolyte is not wider than the potential difference between the positive and negative active materials, the electrolyte cannot suppress side reactions of the electrolyte induced at the interface of the electrode active materials.
[0006] However, as the range of applications of secondary batteries expands, there is an increasing demand for batteries that have higher energy density and realize high voltages of 4 V or more. To meet this demand, conventional positive electrodes use high voltage positive electrode active materials, which makes the potential window of the electrolyte narrower than the potential window of the electrode active material.
[0007] To solve this problem, a protective film that prevents direct contact between the electrolyte and the electrode active material can be formed to suppress decomposition of the electrolyte, thereby providing a method for maintaining capacity during long-term cycles.
[0008] As an example, succinonitrile, adiponitrile, glutaronitrile, etc. are used as electrolyte additives for protecting the positive electrode. These are known to realize excellent thermal properties and high temperature performance, and to improve the voltage drop phenomenon during the activation process. In addition, it is known that they increase ionic conductivity and polarity, and the nitrile group forms a strong bond with a transition metal such as cobalt on the surface of the positive electrode, and the metal-ligand bond suppresses various interfacial side reactions, blocking gas generation and micro-short circuit paths. However, as described above, the electrolyte additives have an excellent effect of protecting the surface of the positive electrode active material, but do not form a protective film on the negative electrode active material, so they cannot suppress side reactions between the negative electrode active material and the electrolyte. Therefore, in order to control the reactivity with the negative electrode, an electrolyte additive such as vinylene carbonate can be added separately to realize cell performance.
[0009] On the other hand, electrolyte additives such as vinylene carbonate can reduce the reactivity between the negative electrode and the electrolyte and suppress side reactions of the electrolyte at the negative electrode. However, due to their low oxidation resistance, they tend to generate gas at the positive electrode when operated at high temperature and high voltage for a long period of time.
[0010] Therefore, the reality is that research is needed on electrolytes that not only suppress electrolyte side reactions at the negative electrode, but also have a wide oxidation potential window and improve side reactions at the positive electrode. Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide an electrolyte composition for lithium secondary batteries which not only has a wide oxidation potential window and is improved in side reactions at the positive electrode, but also can be used under high voltage conditions. [Means for solving the problem]
[0012] To solve the above-mentioned problems, In one embodiment, the present invention comprises: The electrolyte includes a non-aqueous organic solvent, a lithium salt, and an electrolyte additive represented by the following chemical formula 1: An electrolyte composition having an oxidation potential window of 4.5 V or higher is provided.
[0013] [ka]
[0014] In the above Chemical Formula 1, R1 is [ka] , [ka] or [ka] and R1' and R1'' are each a hydrogen or a methyl group; R2 is an oxygen atom, a nitrogen atom, a sulfur atom, an arylene group having 6 to 20 carbon atoms, an aryleneoxy group having 6 to 20 carbon atoms, a heteroarylene group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, a heteroaryleneoxy group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, and [ka] Includes one or more of the following: R3 is a fluoro group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or [ka] and The above alkyl groups, alkoxy groups, and cycloalkyl groups, [ka] and [ka] One or more of the hydrogen atoms contained in may be optionally substituted with a fluorine atom; M includes at least one selected from the group consisting of lithium, sodium, potassium, tetraalkylammonium having 1 to 4 carbon atoms, and tetraalkylphosphonium having 1 to 4 carbon atoms; l is an integer from 1 to 6; m and n are each an integer of 2 to 20.
[0015] In this case, the oxidation potential window of the electrolyte composition may be within the range of 5.0V to 6.0V.
[0016] In addition, in the above chemical formula 1, R2 is an ethylene group, a propylene group, a cyclohexylene group, a phenylene group, an oxymethylene group, a pyrrole group, an oxyphenylene group, an oxynaphthalenyl group, an oxypyrrole group, an oxythiophenylene group, an oxyfuranyl group, or [ka] and R3 is a fluoro group, a methyl group, a fluoromethyl group, a methoxy group, a fluoromethoxy group, or [ka] And the above [ka] One or more of the hydrogen atoms contained in may be optionally substituted with a fluorine atom; M can be lithium.
[0017] As an example, the electrolyte additive represented by Chemical Formula 1 may include one or more compounds selected from the following <Structural Formula 1> to <Structural Formula 17>. [ka] [ka]
[0018] In addition, the electrolyte additive represented by Formula 1 may be included in an amount of 10 wt % or less based on the total weight of the electrolyte composition.
[0019] The non-aqueous organic solvent may include an ester solvent represented by the following Chemical Formula 2:
[0020] [ka]
[0021] In the above Chemical Formula 2, [ka] is a single or double bond, X1 and X2 each represent a hydrogen atom, a fluoro group, a methyl group, an ethyl group, a methyl fluoride group, an ethyl fluoride group, or a vinyl group; p is an integer from 1 to 3.
[0022] Specifically, the ester solvent represented by Chemical Formula 2 above may include one or more of dihydrofuranone, vinyldihydrofuranone, fluorodihydrofuranone, furanone, and tetrahydropyranone.
[0023] The non-aqueous organic solvent may further contain at least one auxiliary solvent selected from the group consisting of fluorine-containing ether solvents, fluorine-containing cyclic carbonate solvents, chain carbonate solvents, phosphate solvents, and sulfone solvents.
[0024] In this case, the auxiliary solvent may be contained in an amount of less than 50% by volume based on the total volume of the non-aqueous organic solvent.
[0025] Further, in one embodiment, the present invention provides an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and There is provided a lithium secondary battery comprising the electrolyte composition according to the present invention described above.
[0026] In this case, the positive electrode may include at least one positive electrode active material selected from lithium metal oxides represented by the following Chemical Formula 3 or 4.
[0027] [Chemical formula 3] Li x [Ni y Co z Mn w M 1 v ]O2
[0028] [Chemical formula 4] LiM 2 p Mn q P r O4
[0029] In the above Chemical Formula 3 and Chemical Formula 4, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, and v are 1.0≦x≦1.30, 0.5≦y<1, 0 <z≦0.3、0<w≦0.3、0≦v≦0.1であり、かつy+z+w+v=1であり、 M 2 is Ni, Co or Fe, p is 0.05≦p≦1.0, q is 1-p or 2-p; r is 0 or 1.
[0030] Specifically, the positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2 and LiNi 0.5 Mn 1.5 It may contain one or more of O4.
[0031] The negative electrode may include a first negative electrode active material containing a carbon material and a second negative electrode active material containing a silicon material, and the carbon material may include one or more of natural graphite, artificial graphite, expanded graphite, non-graphitizable carbon, carbon black, acetylene black, and ketjen black.
[0032] The silicon material may be silicon (Si), silicon carbide (SiC), or silicon oxide (SiO q , where 0.8≦q≦2.5) may be included.
[0033] The second negative electrode active material may be included in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode active material. Effect of the Invention
[0034] The electrolyte composition for a lithium secondary battery according to the present invention includes an electrolyte represented by Chemical Formula 1, and has an oxidation potential window at 4.5 V or more, thereby improving the oxidation stability of the electrolyte composition, and has the advantage that decomposition of the electrolyte composition at high voltages can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Because the present invention is susceptible to various modifications and can have various embodiments, specific embodiments are described in detail in the detailed description.
[0036] However, this is not intended to limit the invention to the particular embodiments, but should be understood to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0037] In the present invention, the terms "comprise" and "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, but should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0038] In addition, in the present invention, when a layer, film, region, plate, or other part is described as being "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between. Conversely, when a layer, film, region, plate, or other part is described as being "under" the other part, this includes not only the case where it is "directly under" the other part, but also the case where there is another part in between. In addition, in the present application, being "on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0039] In addition, in the present invention, "containing as a main component" may mean containing 50% by weight or more (or 50% by volume or more), 60% by weight or more (or 60% by volume or more), 70% by weight or more (or 70% by volume or more), 80% by weight or more (or 80% by volume or more), 90% by weight or more (or 90% by volume or more), or 95% by weight or more (or 95% by volume or more) of a defined component based on the total weight (or total volume). For example, "containing graphite as a main component as a negative electrode active material" may mean containing 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or 95% by weight or more of graphite based on the total weight of the negative electrode active material, and in some cases, it may mean that the entire negative electrode active material is made of graphite and contains 100% by weight of graphite.
[0040] The present invention will now be described in more detail.
[0041] <Electrolyte composition for lithium secondary batteries> In one embodiment, the present invention comprises: The electrolyte includes a non-aqueous organic solvent, a lithium salt, and an electrolyte additive represented by the following chemical formula 1: An electrolyte composition having an oxidation potential window of 4.5 V or higher is provided.
[0042] [ka]
[0043] In the above Chemical Formula 1, R1 is [ka] , [ka] or [ka] and R1' and R1'' are each a hydrogen or a methyl group; R2 is an oxygen atom, a nitrogen atom, a sulfur atom, an arylene group having 6 to 20 carbon atoms, an aryleneoxy group having 6 to 20 carbon atoms, a heteroarylene group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, a heteroaryleneoxy group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, and [ka] Includes one or more of the following: R3 is a fluoro group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or [ka] and The above alkyl groups, alkoxy groups, and cycloalkyl groups, [ka] and [ka] One or more of the hydrogen atoms contained in may be optionally substituted with a fluorine atom; M includes at least one of lithium, sodium, potassium, tetraalkylammonium having 1 to 4 carbon atoms, and tetraalkylphosphonium having 1 to 4 carbon atoms; l is an integer from 1 to 6; m and n are each an integer of 2 to 20.
[0044] The electrolyte composition for a lithium secondary battery according to the present invention includes a non-aqueous organic solvent and a lithium salt, as well as an electrolyte additive represented by Chemical Formula 1. The electrolyte additive includes an ionic compound having a mother nucleus in which a vinyl group, a (meth)acrylate group, or an acrylamide group is bonded (i.e., "R1") to a sulfonylimide group on one side thereof via i) a structure including a saturated hydrocarbon chain or an oxygen atom introduced into the saturated hydrocarbon chain, or ii) a structure including a polyglycol unit (i.e., "R2") that extends the conjugation of the sulfonylimide group.
[0045] The electrolyte additive has a vinyl group, a (meth)acrylate group, or an acrylamide group bonded to one side of the sulfonylimide, and between them, i) a structure containing a saturated hydrocarbon chain or an oxygen atom introduced into the saturated hydrocarbon chain, or ii) a linker (R2) having a structure extending the conjugation of the sulfonylimide group or having a polyglycol unit is introduced, so that an organic film and / or an inorganic film can be uniformly formed on the positive and negative electrode surfaces upon activation of the secondary battery. That is, the electrolyte additive can be directly included in the organic film and / or the inorganic film formed on the positive and / or negative electrode surfaces upon activation of the secondary battery in the form of a monomolecular molecule. In addition, the electrolyte additive can increase the oxidation potential window of the electrolyte, thereby suppressing side reactions between the positive and / or negative electrodes and the electrolyte composition. Therefore, the electrolyte additive can expand the oxidation potential window of the electrolyte composition and at the same time improve the electrical performance of the secondary battery containing it.
[0046] For this purpose, in the compound represented by the above chemical formula 1, R2 is an ethylene group, a propylene group, a cyclohexylene group, a phenylene group, an oxymethylene group, a pyrrole group, an oxyphenylene group, an oxynaphthalenyl group, an oxypyrrole group, an oxythiophenylene group, an oxyfuranyl group, or [ka] and R3 is a fluoro group, a methyl group, a fluoromethyl group, a methoxy group, a fluoromethoxy group, or [ka] And the above [ka] One or more of the hydrogen atoms contained in may be optionally substituted with a fluorine atom; M is lithium, l is an integer of 1 or 2, and m can be an integer from 2 to 10.
[0047] As an example, the compound represented by Chemical Formula 1 above may be one or more of the compounds represented by the following <Structural Formula 1> to <Structural Formula 17>. [ka] [ka]
[0048] The electrolyte additives represented by the above structural formulas 1 to 17 can uniformly form organic / inorganic coating layers on the surfaces of the positive and negative electrodes during activation of a secondary battery. In addition, the electrolyte additives can easily increase the oxidation potential window of the electrolyte composition, thereby effectively suppressing side reactions between the electrodes and the electrolyte during charging and discharging of the secondary battery.
[0049] As one example, the electrolyte composition according to the present invention may have an oxidation potential window of 4.5 V or more. More specifically, the oxidation potential window of the electrolyte composition may be within a range of 4.5 V to 7.0 V, 5.0 V to 6.5 V, 5.0 V to 6.0 V, 5.3 V to 6.5 V, or 5.5 V to 6.0 V.
[0050] The oxidation potential window is a voltage range in which no additional electrochemical reactions occur inside the secondary battery other than the electrochemical oxidation and reduction that occurs between the positive and negative electrodes. The oxidation potential window may be a value measured when a lithium electrode is used as a reference electrode, and thus Li / Li + The oxidation potential window of the electrolyte may mean a relative value to the potential window. In the present invention, when the oxidation potential window of the electrolyte is out of the above range, the potential window becomes narrow, and therefore the non-aqueous electrolyte itself undergoes electrolysis upon charging and discharging the battery, shortening the life of the lithium secondary battery, and there is a problem that a safety problem occurs due to the generated gas. In addition, when the electrolyte composition according to the present invention satisfies the above-mentioned oxidation potential window range, the stability against the potential applied during charging and discharging of the secondary battery can be improved. As a result, the lithium secondary battery containing the electrolyte composition can not only have an improved battery life, but also reduce the risk of explosion and the like.
[0051] In addition, the electrolyte additive may be included in a specific content in the electrolyte composition. Specifically, the electrolyte additive including the compound represented by Chemical Formula 1 may be included in an amount of 10 wt % or less based on the total weight of the electrolyte composition, specifically, 0.01 wt % to 5 wt %, more specifically, 0.05 wt % to 3 wt %, or 1.0 wt % to 2.5 wt % based on the total weight of the electrolyte composition. The present invention can prevent the electrolyte additive from being used in an excessive amount, which causes an increase in the viscosity of the electrolyte composition to decrease the wettability of the electrodes and the separator, and can prevent the electrolyte additive from being used in an excessive amount, which causes an decrease in the ion conductivity of the electrolyte composition to decrease the battery performance. In addition, the present invention can prevent the electrolyte additive from being used in an excessive amount outside the above range, which causes the additive to be ineffectively realized.
[0052] The electrolyte composition according to the present invention is a liquid electrolyte and includes a lithium salt and a non-aqueous organic solvent. In this case, the non-aqueous organic solvent may include an ester-based solvent represented by the following formula 2 as a main component for a synergy effect with the electrolyte additive.
[0053] [ka]
[0054] In the above Chemical Formula 2, [ka] is a single or double bond, X1 and X2 each represent a hydrogen atom, a fluoro group, a methyl group, an ethyl group, a methyl fluoride group, an ethyl fluoride group, or a vinyl group; p is an integer from 1 to 3.
[0055] As an example, the ester solvent represented by Chemical Formula 2 may include one or more of the ester compounds shown below. [ka]
[0056] The ester-based compound itself realizes a lower oxidation potential window of the electrolyte composition compared to a carbonate-based solvent. However, when the ester-based compound is used in combination with the electrolyte additive represented by Chemical Formula 1, not only is the oxidation potential window excellent in expandability, but the stability of the electrolyte is further improved, and the amount of gas generation at high temperature and / or high voltage can be reduced.
[0057] In addition, the non-aqueous organic solvent may further include one or more auxiliary solvents selected from the group consisting of fluorine-containing ether solvents, fluorine-containing cyclic carbonate solvents, chain carbonate solvents, phosphate solvents, and sulfone solvents, in addition to the ester solvent described above.
[0058] Specifically, the fluorine-containing ether solvent may be 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), and the fluorine-containing cyclic carbonate solvent may be fluoroethylene carbonate (FEC). The chain carbonate solvent may be ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and the phosphate solvent may be trimethyl phosphate (TMP), tris(2-ethylhexyl) phosphate, and the sulfone solvent may be sulfolane, methyl sulfolane, dimethyl sulfoxide, sulfonamide, and the like.
[0059] From the viewpoints of electrochemical stability against oxidation-reduction and chemical stability with respect to reactions with heat or solutes, the above auxiliary solvents may be used alone in a mixture with the ester-based solvent, or two or more kinds may be used in any combination in accordance with the application in a mixture with the ester-based solvent.
[0060] In addition, the auxiliary solvent may be mixed with the ester solvent to satisfy a certain volume ratio. Specifically, the auxiliary solvent may be contained in an amount of less than 50% by volume based on the total volume of the non-aqueous organic solvent, and more specifically, the auxiliary solvent may be contained in an amount of 40% by volume or less, 30% by volume or less, 20% by volume or less, 1% to 30% by volume, 1% to 20% by volume, 5% to 20% by volume, 10% to 20% by volume, or 20% to 30% by volume based on the total volume of the non-aqueous organic solvent.
[0061] By adjusting the content of the auxiliary solvent in the entire non-aqueous organic solvent to the above ratio, the present invention can maintain high compatibility between the ester solvent and the auxiliary solvent, and at the same time, can improve the charge mobility and / or ion mobility of the battery, thereby improving the performance of the battery.
[0062] In addition, the non-aqueous organic solvent may be mixed with a solvent used in the art for non-aqueous electrolytes, and the amount of the non-aqueous organic solvent may be less than 10% by weight based on the total weight of the non-aqueous organic solvent. Examples of the non-aqueous organic solvent that can be mixed include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate (EC), propylene carbonate, butylene carbonate, 1,2-dimethoxyethane (DME), tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0063] Meanwhile, the lithium salt may be used without any particular limitation as long as it is used in the art for non-aqueous electrolytes. Specifically, the lithium salt may be LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, (FSO2)2NLi, LiBF2(C2O4)(LiODFB), LiTDI, C4F2LiO8P(LiDFOP), and LiF2NO4S2(LiFSI).
[0064] There is no particular limit to the concentration of these lithium salts, but the lower limit of the preferred concentration range is 0.5 mol / L or more, specifically 0.7 mol / L or more, more specifically 0.9 mol / L or more, and the upper limit of the preferred concentration range is 2.5 mol / L or less, specifically 2.0 mol / L or less, more specifically 1.5 mol / L or less. If the concentration of the lithium salt is below 0.5 mol / L, the ionic conductivity decreases, which may cause the cycle characteristics and output characteristics of the nonaqueous electrolyte battery to decrease. If the concentration of the lithium salt is above 2.5 mol / L, the viscosity of the electrolyte for the nonaqueous electrolyte battery increases, which may also cause the ionic conductivity to decrease, which may cause the cycle characteristics and output characteristics of the nonaqueous electrolyte battery to decrease.
[0065] In addition, when a large amount of lithium salt is dissolved in a non-aqueous organic solvent at once, the liquid temperature may rise due to the heat of dissolution of the lithium salt. In this way, when the temperature of the non-aqueous organic solvent rises significantly due to the heat of dissolution of the lithium salt, in the case of a lithium salt containing fluorine, decomposition may be promoted and hydrogen fluoride (HF) may be generated. Hydrogen fluoride (HF) is not preferable because it causes deterioration of battery performance. Therefore, the temperature when dissolving the lithium salt in the non-aqueous organic solvent is not particularly limited, but may be adjusted to -20°C to 80°C, specifically, 0°C to 60°C.
[0066] The electrolyte composition may further contain additives in addition to the basic components described above. As long as the gist of the present invention is not impaired, additives generally used in the nonaqueous electrolyte of the present invention may be added at any ratio. Specifically, additives such as cyclohexylbenzene, biphenyl, t-butylbenzene, carbonate, vinylethylene carbonate, difluoroanisole, fluoroethylene carbonate, propane sultone, succinonitrile, and dimethylvinylene carbonate may be mentioned. The additives may have an overcharge prevention effect, an anode film formation effect, and a cathode protection effect. In addition, as in the case of use in a nonaqueous electrolyte battery called a lithium polymer battery, it is also possible to use the electrolyte for a nonaqueous electrolyte battery by solidifying it with a gelling agent or a crosslinked polymer.
[0067] <Lithium secondary battery> Further, in one embodiment, the present invention provides an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and There is provided a lithium secondary battery comprising the electrolyte composition according to the present invention described above.
[0068] The lithium secondary battery according to the present invention includes an electrode assembly in which a positive electrode, a separator, and a negative electrode are sequentially arranged, and an electrolyte composition in which a lithium salt and an electrolyte additive are dissolved in a non-aqueous organic solvent. Since the lithium secondary battery includes the electrolyte composition according to the present invention having an expanded oxidation potential window, side reactions such as electrolyte decomposition during operation under high voltage conditions can be improved, and therefore the lithium secondary battery can be usefully applied to fields requiring high voltage operation conditions.
[0069] Each component of the lithium secondary battery will now be described in more detail.
[0070] The electrode assembly includes a positive electrode, a separator, and a negative electrode, where the positive electrode includes a positive electrode mixture layer prepared by applying a slurry containing a positive electrode active material onto a positive electrode current collector, drying, and pressing the slurry, and may further include a conductive material, a binder, and other additives as necessary.
[0071] The positive electrode active material is a material capable of electrochemically reacting on a positive electrode current collector, and may include at least one of lithium metal oxides represented by the following Chemical Formula 3 and Chemical Formula 4 capable of reversibly intercalating and deintercalating lithium ions.
[0072] [Chemical formula 3] Li x [Ni y Co z Mn w M 1 v ]O2
[0073] [Chemical formula 4] LiM 2p Mn q P r O4
[0074] In the above Chemical Formula 3 and Chemical Formula 4, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, and v are 1.0≦x≦1.30, 0.5≦y<1, 0 <z≦0.3、0<w≦0.3、0≦v≦0.1であり、かつy+z+w+v=1であり、 M 2 is Ni, Co or Fe, p is 0.05≦p≦1.0, q is 1-p or 2-p; r is 0 or 1.
[0075] The lithium metal oxides represented by the above formulas 3 and 4 are materials containing high amounts of nickel (Ni) and manganese (Mn), respectively, and when used as a positive electrode active material, have the advantage of being capable of stably supplying high capacity and / or high voltage electricity.
[0076] In this case, the lithium metal oxide represented by the above chemical formula 3 is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co 0.1 Mn 0.1 Al0.1 O2, etc., and the lithium metal oxide represented by the above chemical formula 4 is LiNi 0.7 Mn 1.3 O4, LiNi 0.5 Mn 1.5 O4, LiNi 0.3 Mn 1.7 O4, LiFePO4, LiFe 0.9 Mn 0.1 PO4, LiFe 0.7 Mn 0.3 PO4, LiFe 0.5 Mn 0.5 PO4, etc., which may be used alone or in combination.
[0077] A positive electrode active material such as lithium iron phosphate oxide (LiFePO4) is difficult to reach the voltage conditions required for forming an organic-inorganic film on the surface of the positive electrode composite layer during the activation process of the battery, and therefore it is difficult to stably form the organic-inorganic film. However, when used as a positive electrode active material, the lithium metal oxides represented by Chemical Formula 3 and Chemical Formula 4 can easily meet the voltage conditions required for forming an organic-inorganic film during the activation process of the battery, and can stably and uniformly form an organic-inorganic film on the positive electrode surface. In addition, the organic-inorganic film thus formed can suppress the oxidation of the electrolyte composition induced on the positive electrode surface.
[0078] The positive electrode active material may be included in an amount of 85 parts by weight or more, specifically 90 parts by weight or more, 93 parts by weight or more, or 95 parts by weight or more, based on the weight of the positive electrode mixture layer.
[0079] The positive electrode mixture layer may further contain a conductive material, a binder, other additives, and the like in addition to the positive electrode active material.
[0080] At this time, the conductive material is used to improve the electrical performance of the positive electrode, and may be one commonly used in the art. Specifically, the conductive material may include at least one selected from natural graphite, artificial graphite, carbon black, acetylene black, denka black, ketjen black, super P, channel black, furnace black, lamp black, thermal black, graphene, and carbon nanotubes.
[0081] The conductive material may be included in an amount of 0.1 to 5 parts by weight based on the weight of each positive electrode composite layer, specifically 0.1 to 4 parts by weight, 2 to 4 parts by weight, 1.5 to 5 parts by weight, 1 to 3 parts by weight, 0.1 to 2 parts by weight, or 0.1 to 1 part by weight.
[0082] In addition, the binder plays a role of binding the positive electrode active material, the positive electrode additive, and the conductive material to each other, and may be used without any particular limitation as long as it has such a function. Specifically, the binder may include one or more resins selected from polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0083] The binder may be included in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 1 to 5 parts by weight, based on the weight of each positive electrode mixture layer.
[0084] The total thickness of the positive electrode mixture layer is not particularly limited, but may be specifically 50 μm to 300 μm, more specifically 100 μm to 200 μm, 80 μm to 150 μm, 120 μm to 170 μm, 150 μm to 300 μm, 200 μm to 300 μm, or 150 μm to 190 μm.
[0085] In addition, the positive electrode may use a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, the positive electrode current collector may use stainless steel, aluminum, nickel, titanium, baked carbon, etc. In the case of using aluminum or stainless steel as the positive electrode current collector, it is also possible to use a current collector that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the average thickness of the current collector may be preferably 3 μm to 500 μm, taking into consideration the conductivity and total thickness of the positive electrode to be manufactured.
[0086] Furthermore, the negative electrode, like the positive electrode, includes a negative electrode mixture layer produced by applying a negative electrode active material onto a negative electrode current collector, drying and pressing the negative electrode active material, and may further selectively include a conductive material, a binder, other additives, and the like as necessary.
[0087] The negative electrode active material may include a carbon material. Specifically, the carbon material means a material mainly composed of carbon atoms, and such a carbon material may include one or more selected from natural graphite, artificial graphite, expanded graphite, non-graphitizable carbon, carbon black, acetylene black, and ketjen black.
[0088] The negative electrode active material may further include a silicon material together with the carbon material. The silicon material means a material mainly composed of silicon atoms. Such silicon materials may include silicon (Si), silicon carbide (SiC), silicon monoxide (SiO), or silicon dioxide (SiO2) alone or in combination. When silicon monoxide (SiO) and silicon dioxide (SiO2) are uniformly mixed or composited as silicon (Si)-containing materials and included in the negative electrode composite layer, they are referred to as silicon oxide (SiO q, where 0.8≦q≦2.5).
[0089] In addition, the silicon material may be included in an amount of 1 wt% to 20 wt% based on the total weight of the negative electrode active material, specifically, 3 wt% to 10 wt%, 8 wt% to 15 wt%, 13 wt% to 18 wt%, or 2 wt% to 8 wt%. By adjusting the content of the silicon material within the above content range, the present invention can maximize the energy density of the battery.
[0090] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery. For example, the negative electrode current collector may be made of copper, stainless steel, nickel, titanium, baked carbon, etc. In the case of the negative electrode current collector being made of copper or stainless steel, it may also be surface-treated with carbon, nickel, titanium, silver, etc. In addition, the average thickness of the negative electrode current collector may be suitably applied to be 1 μm to 500 μm, taking into consideration the conductivity and total thickness of the negative electrode to be manufactured.
[0091] Meanwhile, the separator interposed between the positive and negative electrodes of each unit cell means an insulating thin film having high ion permeability and mechanical strength. The separator may be any commonly used in the art, and may be one or more of polypropylene, polyethylene, and polyethylene-propylene copolymers that are chemically resistant and hydrophobic. The separator may have a porous polymer substrate such as a sheet or nonwoven fabric containing the above-mentioned polymer, and may have a composite separator formed by coating organic or inorganic particles on the porous polymer substrate with an organic binder. The separator may have an average pore diameter of 0.01 μm to 10 μm and an average thickness of 5 μm to 300 μm.
[0092] Meanwhile, the lithium secondary battery according to the present invention is not particularly limited, but may be variously applied to a cylindrical shape, a square shape, a pouch type, a coin type, etc. according to the purpose. The lithium secondary battery according to an embodiment of the present invention may be a pouch type secondary battery.
[0093] The present invention will now be described in more detail with reference to examples and experimental examples.
[0094] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0095] <Examples 1 to 25 and Comparative Examples 1 to 4. Production of electrolyte compositions for lithium secondary batteries> A non-aqueous electrolyte composition for a lithium secondary battery was prepared by weighing the electrolyte additive based on the weight of the entire electrolyte composition and mixing it with a non-aqueous solvent in which LiPF6 was dissolved at 1 M. The type of lithium salt, the composition of the non-aqueous solvent, and the type and content of the electrolyte additive are as shown in Table 1 below.
[0096] [Table 1A] [Table 1B]
[0097] <Comparative Example 5. Production of electrolyte composition for lithium secondary battery> A non-aqueous electrolyte composition for a lithium secondary battery was prepared by carrying out the same method as in Example 1, except that an oligomer (weight average molecular weight: 2,500 to 5,000) obtained by polymerizing a compound represented by Structural Formula 1 was used instead of the compound represented by Structural Formula 1 as an electrolyte additive.
[0098] <Examples 26 to 50 and Comparative Examples 6 to 10. Production of Lithium Secondary Batteries> The positive electrode active material is LiNi with a particle size of 5 μm. 0.7 Co 0.1Mn 0.1 Al 0.1 O2 was prepared and mixed with polyvinylidene fluoride as a carbon-based conductive material and binder in N-methylpyrrolidone (NMP) in a weight ratio of 94:3:3 to form a slurry, which was then cast onto an aluminum sheet, dried in a vacuum oven at 120°C, and rolled to produce a positive electrode.
[0099] Separately, a negative electrode active material in which natural graphite and artificial graphite were mixed in a weight ratio of 1:1 was prepared, and 97 parts by weight of the negative electrode active material and 3 parts by weight of styrene-butadiene rubber (SBR) were mixed with water to form a slurry. The slurry was cast on a copper sheet, dried in a vacuum oven at 130°C, and then rolled to produce a negative electrode.
[0100] A separator made of 18 μm polypropylene was placed between the positive electrode and the negative electrode obtained above, and the electrodes were inserted into a case. The electrolyte compositions prepared in the above Examples and Comparative Examples were then injected as shown in Table 2 below to assemble a lithium secondary battery.
[0101] Each assembled lithium secondary battery was initially charged. Specifically, the lithium secondary battery was initially charged under the conditions shown in Table 2 below at 55±2° C. to a charge cut-off voltage of 4.2 V to produce an activated lithium secondary battery.
[0102] [Table 2]
[0103] <Experimental Example 1.> In order to evaluate the performance of the electrolyte composition according to the present invention, the following experiments were carried out on the electrolyte compositions used in the Preparation Examples and Comparative Examples.
[0104] a) Cyclic voltammetry (CV) evaluation of three-electrode battery First, in order to confirm that a coating layer was formed on the surface of the positive electrode, the electrolyte compositions used in Examples 1 to 25 and Comparative Examples 1 to 5 were injected into batteries including a platinum electrode, a platinum electrode, and a lithium metal electrode as three electrodes to fabricate three-electrode batteries, and cyclic voltammetry (CV) analysis was performed on each of the fabricated batteries. At this time, cyclic voltammetry (CV) was performed under conditions of 60°C, an observation range of 3.0V to 6.0V (lithium standard), and a measurement speed of 10mV / s. In addition, lithium (Li / Li + ) the potential at which the electrolyte composition was oxidatively decomposed was calculated, and the results are shown in Table 3 below.
[0105] [Table 3]
[0106] As shown in Table 3, it was confirmed that the electrolyte composition according to the present invention contains an electrolyte additive represented by Chemical Formula 1, and thus the oxidation potential window is expanded. Specifically, the electrolyte composition of the Example contains an electrolyte additive, and the current increases at about 5.15±0.05 V or more. In contrast, the electrolyte compositions of the Comparative Examples, which do not contain an electrolyte additive or contain an electrolyte additive different from the present invention, show an increase in current at 4.90±0.05 V or less.
[0107] Such an increase in current indicates that oxidative decomposition of the electrolyte occurs, forming an organic-inorganic coating layer on the surface of the positive electrode. That is, the electrolyte composition of the above example contains the electrolyte additive represented by Chemical Formula 1, and thus the oxidation potential window is expanded by about 0.25 V or more compared to the electrolyte composition of the comparative example. These results show that the electrolyte composition according to the present invention has improved oxidation stability.
[0108] B) Differential capacity curve analysis of half-cell In order to confirm the action of the electrolyte composition according to the present invention on the surface of the negative electrode, a half-cell was prepared using lithium metal and graphite (a mixture of artificial graphite and natural graphite in a weight ratio of 9:1), and the electrolyte compositions prepared in Examples 1 to 25 and Comparative Examples 1 to 5 were injected into the half-cell. Then, the half-cell was charged at 25° C. and 3.5±0.5 V at a rate of 0.005 C to 0.05 V, and the potential value (V) and capacity value (mAh) were measured, and the potential value was differentiated from the capacity value (dQ / dV) to calculate the reduction potential value.
[0109] As a result, it was confirmed that the electrolyte composition of the Example containing the electrolyte additive represented by Chemical Formula 1 according to the present invention showed a downward peak at a voltage of about 1.32 V relative to lithium, unlike the electrolyte composition of the Comparative Example not containing an electrolyte additive. The downward peak means that a reduction reaction occurred on the surface of the graphite electrode, which is the negative electrode, and indicates that the electrolyte additive represented by Chemical Formula 1 contained in the electrolyte composition is converted into a coating material by a reduction reaction on the surface of the negative electrode at about 1.32 V relative to lithium.
[0110] From these results, it can be seen that in the lithium secondary battery according to the present invention, a reduction reaction is induced on the surface of the negative electrode during the activation process, and an organic / inorganic coating layer is formed.
[0111] <Experimental Example 2.> In order to evaluate the oxidation stability of the electrolyte composition according to the present invention under high temperature and high voltage conditions, the high rate discharge capacity and gas generation amount were measured for the lithium secondary batteries produced in Examples 26 to 50 and Comparative Examples 6 to 10.
[0112] Specifically, the lithium secondary batteries of Examples 26 to 50 and Comparative Examples 6 to 10 were each charged at 25° C. under CC-CV conditions to 4.2 V at a rate of 0.33 C, and then discharged under CC conditions to 2.5 V at a rate of 0.33 C to activate them. Thereafter, each activated lithium secondary battery was charged under CC-CV conditions at a rate of 0.33 C to 4.5 V, and then discharged under CC conditions at a rate of 0.33 C to 2.5 V. The above charge and discharge constitute one cycle, and three charge and discharge cycles were performed.
[0113] The volume of the secondary battery was then measured using Archimedes' principle. The battery was then fully charged at 60°C at a rate of 0.33C to 4.5V under CC-CV conditions, and discharged at a rate of 2.5C to 2.5V under CC conditions to measure the high-rate discharge capacity at high temperature. After the measurement of the high-rate discharge capacity was completed, the volume of the secondary battery was measured in the same manner as the previous volume measurement, and the volume change was calculated. At this time, the volume change was determined to mean the amount of gas generated during high-temperature / high-rate charge / discharge. The results are shown in Table 4 below.
[0114] [Table 4]
[0115] The lithium secondary battery according to the present invention contains the electrolyte composition of the present invention with an expanded oxidation potential window and has excellent oxidation stability, and therefore exhibits excellent battery performance under high temperature and high voltage conditions.
[0116] Specifically, it was confirmed that the lithium secondary battery manufactured in the examples includes an electrolyte composition containing an electrolyte additive represented by Chemical Formula 1, and exhibits a high discharge capacity of 665 mAh or more under high temperature and high voltage conditions. In particular, when the electrolyte composition of the lithium secondary battery in the examples contains an ester-based organic solvent, the amount of gas generated by decomposition of the electrolyte composition during charging and discharging was low at less than 1900 μl.
[0117] From these results, it can be seen that the lithium secondary battery according to the present invention contains an electrolyte represented by Chemical Formula 1, contains an electrolyte composition having an oxidation potential window of 4.5 V or more, and exhibits excellent electrical performance even under high temperature and / or high voltage conditions.
[0118] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood by those skilled in the art or those having ordinary knowledge in the art that the present invention may be modified and changed in various ways without departing from the spirit and technical scope of the present invention as described in the claims below.
[0119] Therefore, the technical scope of the present invention should not be limited to the contents described in the Summary of the Invention of the specification, but should be defined by the claims.
Claims
1. The electrolyte includes a non-aqueous organic solvent, a lithium salt, and an electrolyte additive represented by the following chemical formula 1: The oxidation potential window is 4.5 V or more, 【Chemistry 1】 In the above Chemical Formula 1, R 1 teeth 【Chemistry 2】 、 【Chemistry 3】 or 【Chemistry 4】 and R 1 ' and R 1 '' are hydrogen or a methyl group, R 2 represents an oxygen atom, a nitrogen atom, a sulfur atom, an arylene group having 6 to 20 carbon atoms, an aryleneoxy group having 6 to 20 carbon atoms, a heteroarylene group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, a heteroaryleneoxy group having 5 to 10 carbon atoms containing one or more heteroatoms selected from N, S, and O, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, and 【Chemistry 5】 Contains one or more of the following: R 3 represents a fluoro group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or 【Chemistry 6】 and The alkyl group, the alkoxy group, the cycloalkyl group, 【Chemistry 7】 and 【Chemistry 8】 At least one of the hydrogen atoms contained in is selectively replaced with a fluorine atom, M includes at least one of lithium, sodium, potassium, tetraalkylammonium having 1 to 4 carbon atoms, and tetraalkylphosphonium having 1 to 4 carbon atoms; l is an integer from 1 to 6; The electrolyte composition, wherein m and n are each an integer from 2 to 20.
2. The electrolyte composition according to claim 1, wherein the oxidation potential window is within a range of 5.0V to 6.0V.
3. R 2 is an ethylene group, a propylene group, a cyclohexylene group, a phenylene group, an oxymethylene group, a pyrrole group, an oxyphenylene group, an oxynaphthalenyl group, an oxypyrrole group, an oxythiophenylene group, an oxyfuranyl group, or 【Chemistry 9】 and R 3 is a fluoro group, a methyl group, a methyl fluoride group, a methoxy group, a methoxy fluoride group, or 【Chemistry 10】 and 【Chemistry 11】 At least one of the hydrogen atoms contained in is selectively replaced with a fluorine atom, 2. The electrolyte composition of claim 1, wherein M is lithium.
4. The electrolyte composition according to claim 1, wherein the electrolyte additive represented by Chemical Formula 1 includes at least one compound selected from the following <Structural Formula 1> to <Structural Formula 17>. 【Chemistry 12】 【Chemistry 13】
5. The electrolyte composition according to claim 1 , wherein the electrolyte additive represented by Formula 1 is contained in an amount of 10 wt % or less based on the total weight of the electrolyte composition.
6. The non-aqueous organic solvent includes an ester solvent represented by the following Chemical Formula 2: 【Chemistry 14】 In the above Chemical Formula 2, 【Chemistry 15】 is a single or double bond, X 1 and X 2 are each a hydrogen atom, a fluoro group, a methyl group, an ethyl group, a methyl fluoride group, an ethyl fluoride group, or a vinyl group, The electrolyte composition according to claim 1, wherein p is an integer of 1 to 3.
7. 7. The electrolyte composition according to claim 6, wherein the ester solvent represented by Chemical Formula 2 includes at least one of dihydrofuranone, vinyldihydrofuranone, fluorodihydrofuranone, furanone, and tetrahydropyranone.
8. The electrolyte composition according to any one of claims 1 to 7, wherein the non-aqueous organic solvent further contains one or more auxiliary solvents selected from the group consisting of fluorine-containing ether solvents, fluorine-containing cyclic carbonate solvents, chain carbonate solvents, phosphate solvents, and sulfone solvents.
9. The electrolyte composition according to claim 8 , wherein the auxiliary solvent is contained in an amount of less than 50% by volume based on the total volume of the non-aqueous organic solvent.
10. an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and A lithium secondary battery comprising the electrolyte composition according to claim 1.
11. The positive electrode includes at least one positive electrode active material selected from lithium metal oxides represented by the following Formula 3 or Formula 4: [Chemical formula 3] Li x [Ni y Co z Mn w M 1 v ]O 2 [Chemical formula 4] LiM 2 p Mn q P r O 4 In the above Chemical Formula 3 and Chemical Formula 4, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w and v are each in the range of 1.0≦x≦1.30, 0.5≦y<1, 0<z≦0.3, 0<w≦0.3, 0≦v≦0.1, and y+z+w+v=1; M 2 is Ni, Co or Fe, p is 0.05≦p≦1.0, q is 1-p or 2-p; The lithium secondary battery according to claim 10 , wherein r is 0 or 1.
12. The positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O 2 , LiNi 0.6 Co 0.2 Mn 0.2 O 2 , LiNi 0.9 Co 0.05 Mn 0.05 O 2 , LiNi 0.6 Co 0.2 Mn 0.1 A 0.1 O 2 , LiNi 0.6 Co 0.2 Mn 0.15 A 0.05 O 2 , LiNi 0.7 Co 0.1 Mn 0.1 A 0.1 O 2 and LiNi 0.5 Mn 1.5 O 4 The lithium secondary battery according to claim 11, comprising one or more of the following:
13. the negative electrode includes a first negative electrode active material containing a carbon material and a second negative electrode active material containing a silicon material; The lithium secondary battery according to claim 10, wherein the carbon material comprises at least one of natural graphite, artificial graphite, expanded graphite, non-graphitizable carbon, carbon black, acetylene black, and ketjen black.
14. The silicon materials include silicon (Si), silicon carbide (SiC) and silicon oxide (SiO q The lithium secondary battery according to claim 13, wherein q is selected from the group consisting of 0.8≦q≦2.
5.
15. The lithium secondary battery of claim 13, wherein the second negative electrode active material is included in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode active material.
Citation Information
Patent Citations
Electrolytic solution for nonaqueous electrolyte battery, and nonaqueous electrolyte battery arranged by use thereof
JP2016157679A
Solid polymer electrolyte comprising a polyalkene carbonate
WO2021013741A1