- 2023-08-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-08-30
AI Technical Summary
The excessive precipitation of chlorine gas in vanadium redox flow batteries due to high concentrations of chloride ions in the electrolyte leads to corrosion of battery materials and increases the risk of system failure, particularly at high temperatures and high state of charge (SOC).
The electrolyte composition is optimized by maintaining specific concentration ratios of chloride ions, sulfate ions, and vanadium ions within the range of 2.9≦[c(Cl - )+c(SO 4 2- )]/c(V n+ )≦3.6, along with the inclusion of phosphate or phosphite ions and additives like -OH, -COOH, or -NH functional groups, to control chlorine gas precipitation and stabilize the electrolyte at wider temperature ranges.
This solution significantly reduces chlorine gas production, protects electrode materials, extends the safe operating temperature range, and enhances energy density and efficiency of the battery system, thereby reducing the need for auxiliary equipment and lowering overall costs.
Smart Images

Figure 2024544449000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to a Chinese patent application bearing application number 202211446542.2 and entitled "Electrolyte and Vanadium Redox Flow Battery" filed with the China Patent Office on November 21, 2022, the entire contents of which are incorporated herein by reference.
[0002] The present application belongs to the technical field of electrolyte preparation, and specifically relates to an electrolyte and a vanadium redox flow battery. [Background technology]
[0003] Vanadium redox flow battery is a redox flow battery in which vanadium ions of different valences are used as positive and negative active materials, and the active materials are dissolved in the supporting electrolyte and are in a liquid circulation flow state. As a new type of energy storage battery, vanadium redox flow battery has the characteristics of large capacity, high safety, long life, resource saving, etc., and can be widely applied in fields such as renewable energy generation, power grid peak adjustment, smart microgrid, and standby power supply. The electrolyte is the storage carrier of electric energy in the vanadium redox flow battery system, and its performance directly affects the indexes such as the electrode life, energy density and efficiency, and system cost of the system, and is related to the reliability of the battery system.
[0004] The long-term stable operation of a vanadium redox flow battery system depends on two factors: the stability of the battery material and the stability of the electrolyte. Frequent operation of the battery at high SOC (overcharging) may cause the system electrode materials to oxidize and lose conductivity. High SOC electrolytes are prone to crystallization or precipitation at high temperatures. For electrolytes containing high concentrations of HCl, the precipitation of a large amount of Cl2 will aggravate the corrosion of battery-related materials and increase the danger of the system environment, so it is a problem to be solved to rationally control the generation of chlorine gas during battery operation. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides an electrolyte, and adjusts the concentration of chloride ions in the electrolyte to control the amount of chloride gas deposition, thereby solving the problem of excessive chloride gas deposition. Another object of the present invention is to provide a vanadium redox flow battery including the electrolyte. [Means for solving the problem]
[0006] In a first aspect, an embodiment of the present application provides an electrolyte, the electrolyte including a positive electrode electrolyte and a negative electrode electrolyte, the positive electrode electrolyte and the negative electrode electrolyte including chloride ions, sulfate ions and vanadium ions, and the positive electrode electrolyte and the negative electrode electrolyte both have a chlorine ion content of 3.0≦[c(Cl - )+c(SO4 2- )] / c(V n+ )≦3.6 is satisfied, Here, c(Cl - ) represents the concentration of the chloride ions, and c(SO4 2- ) represents the concentration of the sulfate ion, and c(V n+ ) represents the concentration of the vanadium ions.
[0007] In some embodiments, The above c(Cl - ) is 1.5mol / L≦c(Cl - ) ≦6.5 mol / L, and / or The above c(SO4 2- ) is 0.5mol / L≦c(SO4 2- ) ≦ 5.5 mol / L, and / or The above c(V n+ ) is 1.6mol / L≦c(V n+ )≦2.65 mol / L.
[0008] In some embodiments, the c(Cl - ) and c(SO4 2- ) is 0.4≦c(Cl - ) / c(SO4 2- )≦3.1.
[0009] In some embodiments, the c(Cl - ) and c(V n+ ) is 0.5≦c(Cl - ) / c(V n+ )≦3.0.
[0010] In some embodiments, the positive electrolyte further comprises phosphate ions, and the positive electrolyte has a pH of 2.9≦[c(Cl - )+c(SO4 2- )+c(PO4 3- )] / c(V n+ )≦3.7, Here, c(PO4 3- ) represents the concentration of phosphate ions.
[0011] In some embodiments, the c(PO 3- )teeth, 0.01mol / L≦c(PO4 3- ) ≦0.15 mol / L, and / or 0.02≦c(PO4 3- ) / c(V n+ )≦0.06, and / or [c(Cl - )+c(SO4 2- )+c(PO4 3- )-0.8×c(V n+ )] ≧ 4.2 mol / L, Here, 0.8×c(V n+ ) represents the average molar concentration of acid radical ions bonded to vanadium ions in the positive electrolyte.
[0012] In some embodiments, the anode electrolyte further comprises a phosphite ion, and the anode electrolyte has a pH of 2.9≦[c(Cl - )+c(SO4 2- )+c(PO3 3- )] / c(V n+ )≦3.7, Here, c(PO3 3- ) represents the concentration of phosphite ions.
[0013] In some embodiments, the c(PO 3- )teeth, 0.01mol / L≦c(PO3 3- ) ≦0.15 mol / L, and / or 0.03≦c(PO3 3- ) / c(V n+ )≦0.1, and / or [c(Cl - )+c(SO4 2- )+c(PO3 3- )-1.5×c(V n+ )]≦4.5 mol / L, Here, 1.5 × c(V n+ ) represents the average molar concentration of acid radical ions bonded to vanadium ions in the anode electrolyte.
[0014] In some embodiments, the positive and negative electrolytes further comprise an additive, and the positive and negative electrolytes have a concentration of 2.9≦[c(Cl - )+c(SO4 2- )+c(A)] / c(V n+ )≦3.7, Here, c(A) represents the concentration of the additive.
[0015] In some embodiments, the additive meets at least one of the following characteristics: (a) The concentration c(A) of the additive satisfies 0.02 mol / L≦c(A)≦0.2 mol / L. (b) The additive is one or more additives containing -OH, -COOH, or -NH2 as a functional group.
[0016] In some embodiments, the temperature stabilization range of the electrolyte is from -30 to 60°C.
[0017] In some embodiments, the chloride ions are provided by an acid or salt containing chloride ions, the sulfate ions are provided by an acid or salt containing sulfate ions, and the vanadium ions are provided by a vanadate salt.
[0018] In a second aspect, embodiments of the present application further provide a vanadium redox flow battery comprising the above electrolyte. Effect of the Invention
[0019] Compared with the prior art, the electrolyte of the present application includes a positive electrode electrolyte and a negative electrode electrolyte, and the positive electrode electrolyte and the negative electrode electrolyte include chloride ions, sulfate ions, and vanadium ions. The positive electrode electrolyte and the negative electrode electrolyte both have a cation concentration of 2.9≦[c(Cl - )+c(SO4 2- )] / c(V n+ )≦3.6, where c(Cl - ) represents the concentration of the chloride ions, and c(SO4 2- ) represents the concentration of the sulfate ion, and c(V n+ ) represents the concentration of the vanadium ions. - , SO4 2- , and V n+ When the concentration relationship is appropriate, it can greatly reduce the production rate of Cl2, reduce the corrosiveness to battery materials, and the small amount of precipitated Cl2 can compensate for the oxidation of the electrode carbon felt of the battery, play a protective role for the electrode carbon felt, and reduce the risk level of the operating environment of the chlorine-containing electrolyte. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow diagram showing a manufacturing process of an electrolyte for a vanadium redox flow battery according to an embodiment of the present application. [Diagram 2] 4 shows the state of electrode corrosion after the electrolyte according to Example 1 was used. [Diagram 3] 4 shows the state of electrode corrosion after the electrolyte according to Comparative Example 1 was used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present application provides an electrolyte and a vanadium redox flow battery, and in order to make the objectives, technical solutions and effects of the present application clearer and more precise, the present application will be described in more detail below by way of examples with reference to the drawings. It should be understood that the specific examples described in the present specification are merely for the purpose of illustrating the present application, and are not intended to limit the present application.
[0022] The applicant found that due to high temperatures (temperature inside the container exceeds 50°C in tropical regions), the positive electrode electrolyte is prone to precipitation of V2O5 at high temperatures, and the temperature range in which the electrolyte can be stably used is narrowed, so that auxiliary equipment such as cooling, heating, ventilation, etc. arranged in the battery system consumes power and reduces the overall efficiency of the battery system. Therefore, by expanding the safe operating temperature range of the electrolyte, the deployment cost of the auxiliary equipment and its power consumption can be effectively reduced, and the cost of the battery system can be reduced while improving the overall efficiency. In addition, when the heat exchange equipment breaks down, the high and low temperature resistance of the electrolyte itself is particularly important for the overall stability of the battery system. The higher the concentration of vanadium ions in the electrolyte, the higher the energy density of the corresponding system and the higher the cost performance, but the narrower the safe temperature range and the higher the risk of pentavalent vanadium precipitation at high temperatures. The temperature stable range of the conventional pure sulfuric acid-based electrolyte is narrow, while the mixed acid-based electrolyte of sulfuric acid and hydrochloric acid significantly improves the energy density and generates chlorine gas that is harmful to the operation process of the battery. In addition, Cl2 precipitated by the low pressure in the plateau region is difficult to reversely dissolve in the electrolyte, so the highly volatile HCl in the solution is constantly circulated by the magnetic pump, increasing air binding. When the pump stops, the reactants in the battery are lost and burned up due to overcharging. High concentration Cl -The precipitation rate of Cl2 is accelerated by the pressure applied to the pump, which increases the risk of Cl2 leaking from the system. Therefore, how to reduce the amount of Cl2 precipitation and maintain its high-temperature performance is a problem that needs to be solved for the mixed acid electrolyte. In addition, the excessive HCl concentration of the mixed acid electrolyte aggravates the problem of precipitation of the trivalent solution at the negative electrode at low temperatures (VCl3 crystals are very likely to form), clogging the pipeline and causing the system to fail to operate, which affects the further industrialization of this technology. Therefore, it is an urgent problem to rationally control the precipitation of Cl2 in the electrolyte of the vanadium redox flow battery.
[0023] In accordance with the above-mentioned problems, the present invention provides an electrolyte for a vanadium redox flow battery, the electrolyte including a positive electrode electrolyte and a negative electrode electrolyte, the positive electrode electrolyte and the negative electrode electrolyte including chloride ions, sulfate ions, and vanadium ions, and the positive electrode electrolyte and the negative electrode electrolyte both satisfy the following: 2.9≦[c(Cl - )+c(SO4 2- )] / c(V n+ )≦3.6 is satisfied, Here, c(Cl - ) represents the concentration of the chloride ions, and c(SO4 2- ) represents the concentration of the sulfate ion, and c(V n+ ) represents the concentration of the vanadium ions.
[0024] In some embodiments, c(Cl - ) is 1.5mol / L≦c(Cl - )≦6.5mol / L. - The value of c(Cl) may be any one of 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L, 5.5 mol / L, 6.0 mol / L, and 6.5 mol / L, or a range consisting of any two of these numbers. - The specific numerical values of ) are merely examples, and any value within the range of 1.5 to 6.5 mol / L, or any two numbers within the range, are within the scope of protection of the present application.
[0025] In some embodiments, preferably, c(Cl - ) is 2.5mol / L≦c(Cl - )≦5.5 mol / L, more preferably c(Cl - ) is 3.0 mol / L or less c(Cl - )≦5.0 mol / L, and most preferably c(Cl - ) is 3.5mol / L≦c(Cl - )≦4.5 mol / L.
[0026] In some embodiments, c(SO 2- ) is 0.5mol / L≦c(SO4 2- )≦5.5mol / L, and c(SO4 2- The value of c(SO4) may be any one of 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L, 5.0 mol / L, and 5.5 mol / L, or a range consisting of any two of these numbers. 2- The specific numerical values of ) are merely examples, and any value within the range of 0.5 to 5.5 mol / L, or any two numbers within the range, are within the scope of protection of the present application.
[0027] In some embodiments, preferably, c(SO 2- ) is 1.5mol / L≦c(SO4 2- )≦4.5mol / L, and more preferably, c(SO4 2- ) is 1.5mol / L≦c(SO4 2- )≦3.5 mol / L, and most preferably c(SO4 2- ) is 1.5mol / L≦c(SO4 2- )≦2.5 mol / L.
[0028] In some embodiments, c(V n+ ) is 1.6mol / L≦c(V n+ )≦2.65mol / L, and c(V n+) may be any one of 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2.0 mol / L, 2.1 mol / L, 2.2 mol / L, 2.3 mol / L, 2.4 mol / L, 2.5 mol / L, and 2.6 mol / L, or a range consisting of any two of these numbers. n+ The specific numerical values of are merely examples, and any value within the range of 1.6 to 2.65 mol / L, or any two numbers within the range, are within the scope of protection of the present application.
[0029] In some embodiments, for high SOC, VO2 + The content of VO2 exceeds 90%, resulting in high concentration + is Cl - It reacts with at a specific rate to form Cl2, and the reaction equation is 2VO2 + +2Cl - +4H + →Cl2 + 2VO 2+ +2H2O. Therefore, chlorine gas is generated under high SOC conditions, and Cl - is VO2 + can be made more stable at high temperatures, but 2.9≦[c(Cl - )+c(SO4 2- )] / c(V n+ After being limited by the range of 3.6, the amount of Cl2 generated can be controlled within a certain range, and a certain amount of chlorine gas deposition can compensate for the oxidation of the battery electrode carbon felt to reduce the amount of chlorine gas in the substrate VO during overcharging. 2+ It is possible to avoid the loss of conductivity due to oxidation of the carbon felt electrode caused by insufficient charge. Based on the above principle, the charging open circuit voltage OCV of the battery is extended from 1.50V to 1.54V, and the discharge energy density of the system is improved by more than 20%. In addition, the controlled Cl concentration of 1.5 to 6.5 mol / L is achieved. - Under these high concentrations, it is possible to avoid air binding of the circulation pump due to rapid Cl2 precipitation and environmental risks due to increased air pressure in the system.
[0030] In some embodiments, c(Cl - ) and c(SO42- ) is 0.4≦c(Cl - ) / c(SO4 2- )≦3.1. - ) / c(SO4 2- ) is within the scope of the present application as long as it is any value within the range of 0.4 to 3.1, or any two numbers within the range. - and SO4 2- is an index of mixed acid system, and the proportional relationship between the two indicates the stability of the electrolyte, and Cl - and SO4 2- When these two gases coexist and reach the above proportional relationship, the saturated vapor pressure of HCl can be reduced. On the other hand, SO4 2- and Cl - are Vn + Since the vanadium ion bonds with the single acid radical to form two different salt structures, the structure after bonding with the single acid radical at high temperatures can alleviate the problem of reduced stability of the electrolyte when the solubility limit is reached.
[0031] In some embodiments, c(Cl - ) and c(Vn + ) is 0.5≦c(Cl - ) / c(Vn + )≦3.0. - ) / c(Vn + The value of c(Cl) is within the scope of the present application as long as it is any value within the range of 0.5 to 3.0, or any two numbers within the range. - ) and c(Vn + ) further indicates the situation of chlorine deposition, because the proper Cl - and Vn + In the proportional relationship with Vn in the solution, + Cl bound to - After removing the H, the solution is charged with H to maintain its conductivity and solubility. + remains, further maintaining the battery efficiency and high temperature stability of the battery, and Cl - and V n+ If the proportional relationship with is within the above range, Cl -This gives the compound a strong complexing ability and removes the remaining Cl. - H + and ensure that a certain amount of chlorine gas is deposited, and the electrode is protected by the deposited chlorine gas.
[0032] In some embodiments, the positive electrolyte further comprises phosphate ions, and the positive electrolyte has a pH of 2.9≦[c(Cl - )+c(SO4 2- )+c(PO4 3- )] / c(Vn + )≦3.7, where c(PO4 3- ) represents the concentration of phosphate ions. - , SO4 2- , PO4 3- and Vn + When the above range is satisfied, the electrolyte protects the performance of the electrode and the phosphate ion is Vn + This further increases the stability against phosphate ion and significantly reduces the rate of chlorine gas deposition. + The stabilizing effect on [VO2(H2O)3] + The bond with vanadium inhibits the deprotonation process that occurs at high temperatures. The complexation reaction is as follows:
[0033] [ka]
[0034] In addition, at high temperatures, the Cl content of the electrolyte containing HCl - and VO2 + produces soluble VO2Cl and avoids the production of insoluble V2O5, and satisfies the positive electrode relationship 2.9≦[c(Cl - )+c(SO4 2- )+c(PO4 3- )] / c(V n+Under the control of 0.1% Cl2≦3.7, the low concentration of free HCl can further reduce the Cl2 generation rate, greatly reducing the corrosion resistance requirements for battery materials, and also reducing the operating environment risk level of the electrolyte containing HCl, and further improving the resistance of the battery containing HCl to plateau areas.
[0035] In some embodiments, c(PO4 3- ) is 0.01mol / L≦c(PO4 3- )≦0.15mol / L. c(PO4 3- The value of c(PO4) may be any one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.10 mol / L, 0.11 mol / L, 0.12 mol / L, 0.13 mol / L, 0.14 mol / L, and 0.15 mol / L, or a range consisting of any two numbers therein. 3- The specific numerical values of ) are merely examples, and any value within the range of 0.01 to 0.15 mol / L, or any two numbers within the range, are within the scope of protection of the present application.
[0036] In some embodiments, c(PO4 3- ) is 0.02≦c(PO4 3- ) / c(Vn + )≦0.06. PO4 3- and Vn + By limiting the proportionality with PO4, excessive formation of insoluble VOPO4 precipitates can be avoided, while too low PO4 3- cannot form an effective spatial arrangement and does not provide any protective effect.
[0037] In some embodiments, c(PO4 3- ) is [c(Cl - )+c(SO4 2- )+c(PO4 3- )-0.8×c(V n+ )] ≧ 4.2 mol / L. Here, 0.8 × c(Vn+ ) represents the average molar concentration of the acid radical ions bound to vanadium ions in the positive electrode electrolyte. When the above range is satisfied, after all the acid radicals are bound to vanadium ions, the free acid whose concentration can still be controlled is H + This can ensure the high-temperature solubility, stability and electrical conductivity of the solution.
[0038] In some embodiments, the anode electrolyte further comprises a phosphite ion, and the anode electrolyte has a concentration of 2.9≦[c(Cl - )+c(SO4 2- )+c(PO3 3- )] / c(V n+ )≦3.7, where c(PO3 3- ) represents the concentration of the phosphite ion. + V by concentration 3+ Therefore, when the negative electrode solution satisfies the numerical range of the above relational expression, the Cl bonded to the vanadium ion in the solution is likely to precipitate. - and SO4 2- After removing the free acid radical, the H + must satisfy the above range. In addition, the phosphite ion has a low-temperature effect of stabilizing the trivalent vanadium ion at the negative electrode of the electrolyte, and in the reducing environment of the negative electrode, the phosphite can exist stably without being oxidized.
[0039] In some embodiments, c(PO 3- ) is 0.01mol / L≦c(PO3 3- )≦0.15mol / L. c(PO3 3- The value of c(PO3) may be any one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.10 mol / L, 0.11 mol / L, 0.12 mol / L, 0.13 mol / L, 0.14 mol / L, and 0.15 mol / L, or a range consisting of any two numbers therein. 3-The specific numerical values of ) are merely examples, and any value within the range of 0.01 to 0.15 mol / L, or any two numbers within the range, are within the scope of protection of the present application.
[0040] In some embodiments, c(PO 3- ) is 0.03≦c(PO3 3- ) / c(V n+ )≦0.1. c(PO3 3- ) and c(V n+ ) satisfies the above range, the low-temperature stabilization effect of the phosphite ion is further improved, and excessively high PO3 3- The concentration of the electrolyte increases the viscosity of the negative electrode solution, thereby preventing a decrease in the solution conductivity and an increase in the electrochemical reaction resistance of the battery.
[0041] In some embodiments, c(PO 3- ) is [c(Cl - )+c(SO4 2- )+c(PO3 3- )-1.5×c(V n+ )]≦4.5 mol / L. Here, 1.5×c(V n+ ) represents the average molar concentration of acid radical ions bound to vanadium ions in the negative electrode electrolyte. When the above range is satisfied, the H released by the remaining free acid radicals after all the acid radicals in the solution have bound to vanadium ions is + However, this can be prevented by reducing the amount of vanadium ions present in the solution, so that the amount of vanadium ions present in the solution is not sufficient to affect the stability of the vanadium ions.
[0042] In some embodiments, the positive and negative electrolytes further include an additive, and the positive and negative electrolytes have a concentration of 2.9≦[c(Cl - )+c(SO4 2- )+c(A)] / c(V n+ )≦3.7, where c(A) represents the concentration of the additive.
[0043] In some embodiments, Cl - For an electrolyte system containing Cl -If the concentration is too high, a large amount of Cl2 will be generated, while in some cases the additive cannot be added in the presence of high Cl2 concentrations, because the additive is easily oxidized and decomposed. However, in the present application, the slow generation of Cl2 allows for the safe addition and stabilization of the additive. - The positive electrode Cl2 generation compensation of the electrolyte containing ensures that the positive electrode carbon felt electrode is not oxidized. On the other hand, a high charge amount brings the risk of high temperature precipitation due to an increase in the positive electrode SOC, but this can be stabilized by adding an additive, and the risk of increasing the open circuit voltage can be further avoided.
[0044] In some embodiments, the additive satisfies the following: The concentration c(A) of the additive satisfies 0.02 mol / L≦c(A)≦0.2 mol / L. The value of c(A) may be any one of 0.02 mol / L, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, and 0.2 mol / L, or a range consisting of any two numbers therein. Note that the specific value of c(A) is merely an example, and any value within the range of 0.02 to 0.2 mol / L, or any range consisting of any two numbers therein, falls within the scope of protection of the present application.
[0045] In some embodiments, the additive is one or more additives containing -OH, -COOH, or -NH2 as a functional group. - When the concentration is within the range of 1.5-6.5mol / L, the addition of the additive is effective in maintaining high temperature stability, and the temperature range is wider, so that the operating temperature range of the battery can reach -15℃~60℃. The reason is that -COOH or -NH2 groups can be adsorbed on the surface of vanadium ions or bonded with vanadium ions, forming a structure with a steric effect, enhancing the repulsive force between vanadium ions and making them more dispersed, preventing the collision between vanadium ions, suppressing the occurrence of precipitation, and improving the stability of the electrolyte. The thermal stability mechanism is as follows:
[0046] [ka]
[0047] The increase in the available hydroxyl functional groups -OH provides more active sites for electron transfer, so that the hydroxyl compounds can effectively improve the electrochemical activity of the electrolyte. 2+ / VO2 + The reversibility of the electrode process can be improved by adding -COOH or -NH2 to VO. 2+ / VO2 + The electron mass transfer process in the electrode process can be improved, thereby improving the electrochemical activity, increasing the utilization rate of the electrolyte, and improving the efficiency and overall performance of the battery.
[0048] In some embodiments, additives may include any one or combination of more of glycerin, succinic acid, carbamic acid, methanesulfonic acid, glutamic acid, oxalic acid, and the like.
[0049] In some embodiments, the electrolyte has a temperature stabilization range of -30 to 60° C. The electrolyte has a temperature stabilization range of Cl - It is determined by the concentration of Cl - When the concentration is in the range of 1.5-6.5 mol / L, the temperature stability range of the electrolyte can be extended to -30-60°C, which can greatly save the cost of thermal management equipment, reduce auxiliary power consumption, and improve the energy efficiency of the battery system. Preferably, the temperature stability range of the electrolyte is -15-60°C. The negative electrode electrolyte (trivalent solution) is stable for at least 7 days at an ambient temperature of -15°C. The positive electrode electrolyte (pentavalent solution) is stable for at least 10 days at an ambient temperature of 60°C.
[0050] In some embodiments, the chloride ions are provided by an acid or salt containing chloride ions, the sulfate ions are provided by an acid or salt containing sulfate ions, and the vanadium ions are provided by a vanadate salt.
[0051] In some embodiments, the chloride ions are provided by hydrochloric acid, the sulfate ions are provided by sulfuric acid, and the vanadium ions are provided by multi-stage purified ammonium vanadate.
[0052] Vanadium redox flow battery
[0053] The vanadium redox flow energy storage battery includes a battery stack and an electrolyte storage tank. The battery stack and the electrolyte storage tank are connected by an inlet pipeline and an outlet pipeline, and a circulation pump is provided in the inlet pipeline.
[0054] The battery stack is composed of ion separators, flow guide plates, carbon felt electrodes, flow path frames, and fastening end plates arranged in series at multiple nodes.
[0055] The separator for the battery is as follows:
[0056] Theoretically, H + In order to allow only vanadium ions of different valences to pass through the positive and negative electrode electrolytes and to suppress cross-mixing of vanadium ions of different valences in the positive and negative electrode electrolytes, a cation exchange membrane having good electrical conductivity and selective permeability is preferred, and a fully fluorinated sulfonic acid type ion exchange membrane may also be used. Improving the hydrophilicity, selective permeability, and service life of the ion exchange membrane is one of the means for increasing the efficiency of vanadium batteries.
[0057] Other battery materials are as follows:
[0058] In order to achieve a large capacity of energy storage, vanadium redox flow batteries must necessarily realize the series or parallel connection of several single cells. Therefore, almost all electrodes, except for the end electrodes, must be manufactured as bipolar electrodes. VO2 +Due to the strong oxidation of the electrolyte and the strong acidity of the electrolyte containing sulfuric acid and hydrochloric acid, the electrode material of the vanadium battery must be resistant to strong oxidation and strong acidity, and must also have characteristics such as low resistance, excellent conductivity, high mechanical strength, and good electrochemical activity. The electrode material of the vanadium battery is mainly carbon, such as graphite, carbon cloth, carbon felt, etc. The bipolar plate is mainly composite material, such as conductive polymer, polymer composite material, etc.
[0059] After the materials of each part of the battery stack are assembled in sequence, they are connected to the inlets and outlets of the corresponding positive and negative electrolyte storage tanks to assemble the vanadium redox flow battery.
[0060] Example 1
[0061] Referring to FIG. 1, taking multi-stage purified ammonium vanadate (NH4)x(VO3)y as an example, it is calcined at 750°C for 5 hours to obtain high-purity vanadium pentoxide (V2O5), and then reducing gas (NH4 or H2) is introduced and calcined for 10 hours to obtain vanadium tetroxide (V2O4) or vanadium trioxide (V2O3). These two oxides are mixed in a 1:1 ratio (trivalent and tetravalent oxides each accounting for 50%), and sulfuric acid and hydrochloric acid are added to produce a mixed acid electrolyte used in the positive and negative electrodes of vanadium redox flow batteries.
[0062] Here, the mixed acid electrolyte obtained contains a positive electrode electrolyte and a negative electrode electrolyte, and the positive electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte is controlled to contain 1.9 mol of SO42 - , 3.9 mol Cl - , and 2.0 mol V n+ The control is to include.
[0063] Example 2
[0064] The specific manufacturing method of Example 2 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 was added to the positive electrode electrolyte. 2- , 4.1 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 4.1 mol Cl - , and 2.0 mol V n+ The control is to include.
[0065] Example 3
[0066] The specific manufacturing method of Example 3 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.3 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 4.3 mol Cl - , and 2.0 mol V n+ The control is to include.
[0067] Example 4
[0068] The specific manufacturing method of Example 4 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 4.5 mol Cl - , and 2.0 mol V n+ The control is to include.
[0069] Example 5
[0070] The specific manufacturing method of Example 5 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.7 mol Cl -and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 4.7 mol Cl - , and 2.0 mol V n+ The control is to include.
[0071] Example 6
[0072] The specific manufacturing method of Example 6 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.9 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 4.9 mol Cl - , and 2.0 mol V n+ The control is to include.
[0073] Example 7
[0074] The specific manufacturing method of Example 7 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 5.1 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 5.1 mol Cl - , and 2.0 mol V n+ The control is to include.
[0075] Example 8
[0076] The specific manufacturing method of Example 8 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 5.3 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 5.3 mol of SO4 2- , 4.7 mol Cl - , and 2.0 mol V n+The control is to include.
[0077] Example 9
[0078] The specific manufacturing method of Example 9 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.3 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.0 mol Cl - and 1.8 mol of V n+ The negative electrode electrolyte contains 1.3 mol of SO4 2- , 4.0 mol Cl - , and 1.8 mol of V n+ The control is to include.
[0079] Example 10
[0080] The specific manufacturing method of Example 10 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 1.8 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.0 mol Cl - and 1.8 mol of V n+ The negative electrode electrolyte contains 1.8 mol of SO4 2- , 4.0 mol Cl - , and 2.0 mol V n+ The control is to include.
[0081] Example 11
[0082] The specific manufacturing method of Example 11 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.1 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.0 mol Cl - and 1.8 mol of V n+ The negative electrode electrolyte contains 2.1 mol of SO4 2- , 4.0 mol Cl - , and 2.0 mol V n+ The control is to include.
[0083] Example 12
[0084] The specific manufacturing method of Example 12 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.4 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.0 mol Cl - and 1.8 mol of V n+ The negative electrode electrolyte contains 2.4 mol of SO4 2- , 4.0 mol Cl - , and 2.0 mol V n+ The control is to include.
[0085] Example 13
[0086] The specific manufacturing method of Example 13 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 1.87 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 4.5 mol Cl - , and 1.87 mol of V n+ The control is to include.
[0087] Example 14
[0088] The specific manufacturing method of Example 14 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 1.95 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 4.5 mol Cl - , and 1.95 mol of V n+ The control is to include.
[0089] Example 15
[0090] The specific manufacturing method of Example 15 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl- and 2.05 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 4.5 mol Cl - , and 2.05 mol of V n+ The control is to include.
[0091] Example 16
[0092] The specific manufacturing method of Example 16 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 2.20 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 4.5 mol Cl - , and 2.20 mol of V n+ The control is to include.
[0093] Example 17
[0094] The specific manufacturing method of Example 17 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 2.30 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 4.5 mol Cl - , and 2.30 mol of V n+ The control is to include.
[0095] Example 18
[0096] The specific manufacturing method of Example 18 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 3.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 1.5 mol Cl - and 1.6 mol of V n+ The negative electrode electrolyte contains 3.2 mol of SO4 2- , 1.5 mol Cl -, and 1.6 mol of V n+ The control is to include.
[0097] Example 19
[0098] The specific manufacturing method of Example 19 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.5 mol of SO4 is added to the positive electrode electrolyte. 2- , 6.5 mol Cl - and 2.6 mol of V n+ The negative electrode electrolyte contains 2.5 mol of SO4 2- , 6.5 mol Cl - , and 2.6 mol of V n+ The control is to include.
[0099] Example 20
[0100] The specific manufacturing method of Example 20 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.2 mol of SO4 is added to the positive electrode electrolyte. 2- , 2.5 mol Cl - and 1.60 mol of V n+ The negative electrode electrolyte contains 2.2 mol of SO4 2- , 2.5 mol Cl - , and 2.20 mol of V n+ The control is to include.
[0101] Example 21
[0102] The specific manufacturing method of Example 21 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 4.0 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.5 mol Cl - and 2.65 mol of V n+ The negative electrode electrolyte contains 4.0 mol of SO4 2- , 4.5 mol Cl - , and 2.65 mol V n+ The control is to include.
[0103] Example 22
[0104] The specific manufacturing method of Example 22 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and the positive electrode electrolyte does not contain PO4 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 3.9 mol Cl - , 0.04 mol PO4 3- , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+ The control is to include.
[0105] Example 23
[0106] The specific manufacturing method of Example 23 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and the positive electrode electrolyte is made of PO4 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 3.9 mol Cl - , 0.08 mol PO4 3- , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+ The control is to include.
[0107] Example 24
[0108] The specific manufacturing method of Example 24 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and the positive electrode electrolyte is made of PO4 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 5.3 mol Cl - , 0.12 mol PO4 3- , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+The control is to include.
[0109] Example 25
[0110] The specific manufacturing method of Example 25 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and PO3 is added to the negative electrode electrolyte. 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - , 0.06 mol PO3 3- , and 2.0 mol V n+ The control is to include.
[0111] Example 26
[0112] The specific manufacturing method of Example 26 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and PO3 is added to the negative electrode electrolyte. 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 3.9 mol Cl - , 0.13 mol PO3 3- , and 2.0 mol V n+ The control is to include.
[0113] Example 27
[0114] The specific manufacturing method of Example 27 is the same as that of Example 1, except that the predetermined ON concentration ratio is different and PO3 is added to the negative electrode electrolyte. 3- The positive electrode electrolyte is added with 1.9 mol of SO4 2- , 5.3 mol Cl - , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2-, 5.3 mol Cl - , 0.2 mol PO3 3- , and 2.0 mol V n+ The control is to include.
[0115] Example 28
[0116] The specific preparation method of Example 28 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and glycerol is added as an additive to the positive electrode electrolyte, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , 3.9 mol Cl - , 2.0 mol V n+ , and 0.02 mol of glycerol, and the negative electrode electrolyte contained 1.9 mol of SO4 2- , 3.9 mol Cl - , and 2.0 mol V n+ The control is to include.
[0117] Example 29
[0118] The specific preparation method of Example 29 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and succinic acid is added as an additive to the positive and negative electrolytes, and 1.9 mol of SO4 is added to the positive electrolyte. 2- , 5.3 mol Cl - , 2.0 mol V n+ , and 0.2 mol succinic acid, and the negative electrode electrolyte contained 1.9 mol SO4 2- , 5.3 mol Cl - , 2.0 mol V n+ , and 0.02 mol of succinic acid.
[0119] Example 30
[0120] The specific manufacturing method of Example 30 is the same as that of Example 1, except that the predetermined on concentration ratio is different, and 2.0 mol of SO4 is added to the positive electrode electrolyte. 2- , 4.6 mol Cl - and 2.25 mol of V n+The negative electrode electrolyte contains 2.11 mol of SO4 2- , 4.33 mol Cl - , and 1.8 mol of V n+ The control is to include.
[0121] Comparative Example 1
[0122] The specific manufacturing method of Comparative Example 1 is the same as that of Example 1, except that chlorine is not added, and 1.9 mol of SO4 is added to the positive electrode electrolyte. 2- , and 2.0 mol V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , and 2.0 mol V n+ The control is to include.
[0123] Comparative Example 2
[0124] The specific manufacturing method of Comparative Example 2 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 was added to the positive electrode electrolyte. 2- , 2.5 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 2.5 mol Cl - , and 2.0 mol V n+ The control is to include.
[0125] Comparative Example 3
[0126] The specific manufacturing method of Comparative Example 3 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 1.9 mol of SO4 was added to the positive electrode electrolyte. 2- , 6.5 mol Cl - and 2.0 mol of V n+ The negative electrode electrolyte contains 1.9 mol of SO4 2- , 6.5 mol Cl - , and 2.0 mol V n+ The control is to include.
[0127] Comparative Example 4
[0128] The specific manufacturing method of Comparative Example 4 is the same as that of Example 1, with the difference being that the predetermined on concentration ratio is different, and 0.488 mol of SO4 was added to the positive electrode electrolyte. 2- , 6.898 mol Cl - and 2.56 mol of V n+ The negative electrode electrolyte contains 0.615 mol of SO4 2- , 7.655 mol Cl - , and 1.941 mol of V n+ The control is to include.
[0129] Performance tests were conducted on the electrolyte solutions of Examples 1 to 31 and Comparative Examples 1 to 4, or the electrolyte solutions were used to prepare vanadium redox flow batteries and the performance of the batteries was tested. Specific test data are shown in Tables 1 to 3.
[0130] Here, the testing of the vanadium redox flow battery includes:
[0131] In the battery efficiency test, a 5W single cell was used, and constant current charging + constant voltage charging + constant current discharging mode was adopted, and the current density of the constant current charging was 110mA / cm 2 The cut-off voltage is 1.6 V, then the battery is charged at a constant voltage of 1.6 V until the open circuit voltage of the battery is 1.54 V, and finally the battery is charged at a constant voltage of 110 mA / cm 2 The battery is discharged at a constant current of 1 V down to the cutoff voltage.
[0132] EE = discharge Wh / charge Wh x 100%, CE = discharge Ah / charge Ah x 100%.
[0133] In the Cl2 precipitation rate test, for single cells with different proportional relationships of active materials, NaOH solution was used to collect gas in the upper layer of the positive electrode electrolyte after two charge-discharge cycles, and then ion chromatography was used to measure the Cl2 precipitation rate in the NaOH collected solution. - The concentration is measured and thus the Cl2 production rate per unit time is obtained.
[0134] In the electrode corrosion acceleration test, a 5W single cell was used, and constant current charging + constant voltage charging + constant current discharging mode was adopted, with the current density of the constant current charging being 110mA / cm 2 The cut-off voltage is 1.8 V, then the battery is charged at a constant voltage of 1.8 V until the open circuit voltage of the battery reaches 1.7 V, and finally the battery is charged at a constant voltage of 110 mA / cm 2 The battery is discharged at a constant current of 1 V down to the cutoff voltage.
[0135] After 50 cycles of charging and discharging, at the end of the discharge, the resistance change of the battery is measured using an AC impedance meter, and the battery is opened to observe the corrosion state of the electrodes.
[0136] [Table 1-1]
[0137] [Table 1-2]
[0138] [Table 2-1]
[0139] [Table 2-2]
[0140] [Table 3]
[0141] Referring to Tables 1 and 2, in Examples 1 to 8 and Comparative Examples 1 to 3, when the concentrations of vanadium ions and sulfate ions were constant, the amount of Cl2 generated gradually increased as the concentration of chloride ions increased, while a clear protective effect was brought about for the electrode. Figures 2 and 3 show the electrode corrosion conditions in Comparative Example 1 and Example 1, respectively. As shown in Figures 2 and 3, when chloride ions were not added to the electrolyte, the electrode was severely corroded, while when the chloride ion concentration was 3.9 to 5.3 mol and [c(Cl - )+c(SO4 2- )] / c(V n+ ) is in the range of 2.9 to 3.6, the electrode can be protected under the action of a small amount of generated chlorine gas. However, the chloride ion concentration in the electrolyte is too high and [c(Cl - )+c(SO4 2- )] / c(V n+ ) is out of the range of 2.9 to 3.6, as in Comparative Example 4, the rate of chlorine gas generation becomes too high, air binding occurs, and it becomes difficult to control the chlorine gas in the battery system, adversely affecting the battery performance.
[0142] In contrast to Examples 9 to 12, when the concentrations of vanadium ions and chloride ions are constant, as the sulfate ion concentration increases, the energy density of the battery gradually increases and the energy efficiency improves. When the sulfate ion concentration increases to 2.1 mol / L, the energy density no longer increases significantly and the change in energy efficiency remains almost constant.
[0143] In comparison with Examples 13 to 17, when the concentrations of sulfate ion and chloride ion are constant, the energy density of the battery gradually increases as the vanadium ion concentration increases, but when the vanadium ion concentration reaches 2.2 mol / L, the increasing tendency becomes gentle. Therefore, the increase in viscosity due to the vanadium ion concentration increases the polarization of the solution concentration, making it difficult to further improve the energy density. In addition, according to the energy efficiency, after the vanadium ion concentration reaches 2.1 mol / L, the efficiency reaches an inflection point and starts to decrease.
[0144] Referring to Table 3, for Example 30 and Comparative Example 4, V n+ The concentration is too high, i.e., 2.9 ≤ [c(Cl - )+c(SO4 2- )] / c(V n+ If the range of )≦3.6 is not met, the mass transfer resistance of the solution due to the increase in viscosity will not be able to continue to increase the energy density of the solution. - If the concentration increases further, a large amount of Cl2 will precipitate, causing severe air binding in the circulation pump and making it difficult to operate stably.
[0145] The above describes the electrolyte and vanadium redox flow battery provided in the examples of the present application, and the present application uses specific examples to explain the principles and embodiments of the present application, and the explanation of the above examples is intended to facilitate understanding of the technical solutions and their core ideas of the present application. It should be understood that those skilled in the art may modify the technical solutions described in the above examples or replace some of the technical features with equivalents, and these modifications or replacements do not deviate from the essence of the corresponding technical solutions from the scope of the technical solutions of each example of the present application.
Claims
1. The positive electrode electrolyte and the negative electrode electrolyte include chloride ions, sulfate ions, and vanadium ions, and the positive electrode electrolyte and the negative electrode electrolyte each have a concentration of 2.9≦[c(Cl - ) + c(SO 4 2- ) )] / c(V n+ )≦3.6, Here, c(Cl - ) represents the concentration of the chloride ions, and c(SO 4 2- ) represents the concentration of the sulfate ion, and c(V n+ ) represents the concentration of the vanadium ions; Electrolyte.
2. The c(Cl - ) is 1.5 mol / L ≦ c (Cl - ) ≦6.5 mol / L; The electrolyte solution according to claim 1.
3. The c(Cl - ) is 2.5 mol / L ≦ c (Cl - ) ≦5.5 mol / L; The electrolyte solution according to claim 1.
4. The c(Cl - ) is 3.0 mol / L ≦ c (Cl - ) ≦5.0 mol / L; The electrolyte solution according to claim 1.
5. The c(Cl - ) is 3.5 mol / L ≦ c (Cl - ) ≦4.5 mol / L; The electrolyte solution according to claim 1.
6. The c(Cl - ) and c(V n+ ) is 0.5≦c(Cl - ) / c(V n+ ) ≦ 3.0; The electrolyte solution according to any one of claims 1 to 5.
7. The c(SO 4 2- ) is 0.5 mol / L ≦ c (SO 4 2- ) ≦5.5 mol / L; The electrolyte solution according to any one of claims 1 to 6.
8. Said c(V n+ ) is 1.6 mol / L ≦ c (V n+ ) ≦2.65 mol / L; The electrolyte solution according to any one of claims 1 to 7.
9. The c(Cl - ) and the c(SO 4 2- ) is 0.4≦c(Cl - ) / c(SO 4 2- )≦3.1; The electrolyte solution according to any one of claims 1 to 8.
10. The positive electrode electrolyte further includes a phosphate ion, and the positive electrode electrolyte has a pH of 2.9≦[c(Cl - ) + c(SO 4 2- ) + c(PO 4 3- ) )] / c(V n+ )≦3.7, Here, c (PO 4 3- ) represents the concentration of phosphate ions, The electrolyte solution according to any one of claims 1 to 9.
11. Said c(PO 4 3- ) further satisfy at least one of the following characteristics: The 4 3- )≦00.15mol / 、 b)0.02≦c(PO 4 3- ) / c(V n+ )≦0.06、 c)[c(Cl - )+c(SO 4 2- )+c(PO 4 3- )-0.8×c(V n+ )]≧4.2mol / L、 Here, 0.8 × c (V n+ ) represents the average molar concentration of acid radical ions bound to vanadium ions in the positive electrode electrolyte; The electrolyte solution according to claim 10.
12. The negative electrode electrolyte further includes a phosphite ion, and the negative electrode electrolyte has a pH of 2.9≦[c(Cl - ) + c(SO 4 2- ) + c(PO 3 3- ) )] / c(V n+ )≦3.7, Here, c (PO 3 3- ) represents the concentration of phosphite ions, The electrolyte solution according to any one of claims 1 to 11.
13. Said c(PO 3 3- ) further satisfy at least one of the following characteristics: The 3 3- )≦00.15mol / 、 e)0.03≦c(PO 3 3- ) / c(N n+ )≦0.1、 f)[c(Cl - )+c(SO 4 2- )+c(PO 3 3- )-1.5×c(V n+ )]≦4.5mol / L、 Here, 1.5 × c (V n+ ) represents the average molar concentration of acid radical ions bound to vanadium ions in the negative electrode electrolyte; The electrolyte solution according to claim 12.
14. The positive electrode electrolyte and the negative electrode electrolyte further include an additive, and the positive electrode electrolyte and the negative electrode electrolyte have a pH of 2.9≦[c(Cl - ) + c(SO 4 2- )+c(A)] / c(V n+ )≦3.7, where c(A) represents the concentration of the additive; The electrolyte solution according to any one of claims 1 to 13.
15. The additive satisfies at least one of the following characteristics: g) the concentration c(A) of the additive satisfies 0.02 mol / L≦c(A)≦0.2 mol / L; h) The additive has a functional group of -OH, -COOH or -NH 2 One or more additives containing The electrolyte solution according to claim 14.
16. The temperature stabilization range of the electrolyte is −30 to 60° C. The electrolyte solution according to any one of claims 1 to 15.
17. the chloride ions are provided by an acid or salt containing chloride ions, the sulfate ions are provided by an acid or salt containing sulfate ions, and the vanadium ions are provided by a vanadate salt; The electrolyte solution according to any one of claims 1 to 16.
18. The electrolyte solution according to any one of claims 1 to 17 is included. Vanadium redox flow battery.
Citation Information
Patent Citations
Electrolyte of all-vanadium redox flow battery and preparation method of electrolyte
CN107069066A
Electrolyte and all-vanadium redox flow battery
CN115498232A
Electrolyte for vanadium redox flow type battery
JP1996064223A
Redox flow battery based on a chloride-containing support solution
JP2013543217A
Manufacturing method for electrolyte, electrolyte and manufacturing apparatus for electrolyte
JP2016162524A
Cited By
Method for detecting content of chloride ions in mixed acid group all-vanadium electrolyte
CN120992846A