Ophthalmic lenses and methods for forming ophthalmic lenses - Patents.com
By encapsulating optical microstructures within ophthalmic lenses using a thermoplastic layer and a thermoset layer, the method ensures protection and maintains the optical integrity of the microstructures, addressing the challenge of damage and deformation in existing lenses.
Patent Information
- Application Number
- JP2024532525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-10
- Filing Date
- 2022-12-08
- Publication Date
- 2024-12-09
AI Technical Summary
Existing ophthalmic lenses with optical elements face challenges in providing adequate protection without altering their optical design, as coatings can damage or change the shape of these elements, leading to compromised functionality.
The solution involves forming ophthalmic lenses with encapsulated optical microstructures using a thermoplastic layer with a microstructure pattern, which is then encapsulated by a thermoset layer, ensuring the microstructures maintain their shape and optical integrity during polymerization and subsequent processing.
This method preserves the optical design and functionality of the microstructures by preventing damage and deformation, allowing for effective protection and integration into ophthalmic lenses without altering their optical properties.
Smart Images

Figure 2024545491000001_ABST
Abstract
Description
[Technical field]
[0001] Field of Disclosure SUMMARY The present disclosure relates to ophthalmic lenses having encapsulated optical elements. [Background technology]
[0002] Myopia, also known as near-sightedness or short-sightedness, is an eye condition in which light entering the eye is not focused directly onto the retina. Instead, light entering the eye is focused in front of the retina, causing the image a person views to be in focus or out of focus depending on the distance of the object from the person's eye. For example, if the object is a distant object, the viewed object will be out of focus, while if the object is a close object, the viewed object will be in focus.
[0003] Optical articles such as ophthalmic lenses can be used to correct refractive errors of the eye. Such errors can include myopia, hyperopia, presbyopia, and astigmatism, among others. Some ophthalmic lenses include optical elements, such as microlenses, that can facilitate the correction of these refractive errors. For example, microlenses can provide a positive add value to focus a portion of the incoming light in front of the retina, thereby controlling the progression of myopia.
[0004] Although theoretically valid, in practice, optical elements are often located on the outer lens surface, which therefore has limited protection from damage and is vulnerable to damage. Some lenses include coatings, such as hard coatings or varnishes, integrated into the optical lens to protect the optical elements. However, these coatings may not adequately protect the optical elements. Furthermore, these coatings may change the shape and optical design of the optical elements. For example, the hardening of the hard coating may result in excessive stress on the optical elements. As a result, the optical elements may no longer be able to provide the optical objectives that the optical elements are designed to meet. Summary of the Invention [Problem to be solved by the invention]
[0005] Thus, there is a need in the art for optical articles that are configured to provide adequate protection for optical elements without altering their optical design. [Means for solving the problem]
[0006] The above "Background" description is intended to provide a general overview of the context of the present disclosure. The inventors' work within the scope of the description in the "Background" and aspects of the present specification that may not be considered prior art at the time of filing are not expressly or implicitly admitted as prior art to the present disclosure.
[0007] The present disclosure relates to a method of forming an ophthalmic lens, as defined in the claim set.
[0008] According to one embodiment, the present disclosure further relates to an ophthalmic lens comprising: a first layer, the first layer having a microstructure on a first surface of the first layer, the microstructure on the first surface of the first layer being formed in a pattern, and the material of the first layer being a thermoplastic material; and a second layer formed on the first surface of the first layer, the glass transition temperature of the first layer being higher than the glass transition temperature of the second layer.
[0009] In particular, the material of the second layer is a thermosetting or thermoplastic material.
[0010] According to one embodiment, the present disclosure further relates to a method as defined in the claim set for forming an ophthalmic lens having an encapsulated lenslet, the method comprising: providing a first layer in a cavity of a forming chamber, the first layer having a microstructure on a first surface of the first layer, the microstructure on the first surface of the first layer being formed in a pattern, and a material of the first layer being a thermoplastic material; flowing a second material into the cavity of the forming chamber and contacting the first surface of the first layer; and setting the second material to form a second layer on the first surface of the first layer, the glass transition temperature of the first layer being higher than the glass transition temperature of the second layer.
[0011] According to an embodiment, the present disclosure further relates to a method of forming an ophthalmic lens, the method including: providing a first layer within a cavity of a forming chamber, the first layer having a microstructure on a first surface of the first layer, the microstructure on the first surface of the first layer being formed in a pattern; flowing a thermosetting material into the cavity of the forming chamber and contacting the first surface of the first layer and a second surface of the first layer, the second surface of the first layer being opposite the first surface of the first layer; and curing the thermosetting material to form a second layer on the first surface of the first layer and a third layer on the second surface of the first layer, the glass transition temperature of the first layer being higher than each of the glass transition temperatures of the second layer and the third layer.
[0012] The above paragraphs have been provided by way of a general introduction and are not intended to limit the scope of the following claims. The described embodiments and further advantages will be best understood by referring to the following detailed description in conjunction with the accompanying drawings, in which:
[0013] A more complete understanding of the present disclosure and many of the attendant advantages thereof will be readily obtained as the same becomes better understood by reference to the following detailed description when considered in conjunction with the accompanying drawings, in which: [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic diagram of a forming chamber according to an exemplary embodiment of the present disclosure. [Diagram 2] 1 is a flow diagram of a method of forming an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 3A] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 3B] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 3C] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 3D] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 4A] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 4B] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 5A] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 5B] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 6A] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 6B] 1 is a diagram of a portion of an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 7] 1 is a graphical representation of the overall refractive power average of a microlens of an ophthalmic lens, according to an exemplary embodiment of the present disclosure. [Figure 8] 1 is a flow diagram of a method of forming an ophthalmic lens according to an exemplary embodiment of the present disclosure. [Figure 9] 1 is an optical image of a PC / PMMA composite lens according to one embodiment of the present disclosure. [Figure 10] 1 is an optical image of a PMMA / PC composite lens as a comparative example. [Figure 11A] 1 is an optical image of a PC / Durabio composite lens according to one embodiment of the present disclosure. [Figure 11B] 1 is a graph of the overall refractive power average of the microlenses in each ring of an ophthalmic lens, according to one embodiment of the present disclosure. [Figure 12] 4 is a graphical representation of the overall refractive power average of microlenses of an ophthalmic lens according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms "a" or "an," as used herein, are defined as one or more. The term "plurality," as used herein, is defined as two or more. The term "another," as used herein, is defined as at least two or more. The terms "including" and / or "having," as used herein, are defined as comprising (i.e., open terms). References throughout this document to "one embodiment," "a particular embodiment," "one embodiment," "one implementation," "one example," or similar terms mean that a particular feature, structure, or characteristic described in connection with that embodiment is included in at least one embodiment of the disclosure. Thus, the appearances of such phrases in various places throughout this specification are not necessarily all referring to the same embodiment. Furthermore, particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments, without limitation.
[0016] The terms "wafer" and "laminate" may be used interchangeably to refer to similar structures. Additionally, the terms "optical lens," "ophthalmic lens," and "corrective lens," and their plurals, may be used interchangeably to refer to similar structures.
[0017] The term "about" or "approximately" is defined as close as understood by one of ordinary skill in the art. In one non-limiting embodiment, the term is defined as within 10%, preferably within 5%, more preferably within 1%, and most preferably within 0.5%.
[0018] Recently, efforts to combat myopia progression include providing optical microstructures directly on the surface of corrective lenses. The optical microstructures can be, for example, microlenses that redirect a portion of the incident light to the retina or to a location relative to the retina. To this end, the use of microlenses on the surface of standard single vision lenses to introduce peripheral defocus has been shown to be effective in slowing the progression of myopia. Microlenses are also used in other applications. For example, microlenses are used in digital projectors, imaging devices (e.g., copy machines, cell phone cameras), microscopes (e.g., for uniform illumination, displays, and to improve the light collection efficiency of charge-coupled device arrays), among other applications.
[0019] The optical microstructures may include microlenses or microlenslets, or any other type of structure or element, with a physical Z distortion / height of 0.1 μm to 50 μm, and a width / length of 0.5 μm to 1.5 mm. The structures preferably have a periodic or quasi-periodic layout, but may have randomized positions. Preferred layouts of the microstructures are a grid with a constant grid step, a honeycomb layout, multiple concentric rings, and continuous microstructures (e.g., no spaces between the microstructures). The structures can provide optical wavefront modification in intensity, curvature, or optical deviation, where the wavefront intensity is configured such that the structures can be absorptive and can locally absorb the wavefront intensity in the range of 0% to 100%, the curvature is configured such that the structures can locally modify the wavefront curvature in the range of ±20 diopters, and the optical deviation is configured such that the structures can locally scatter the light at angles in the range of ±1° to ±30°. The distance between structures can range from 0 (continuous) to 3 times the structures (discrete microstructures) in X and / or Y size.
[0020] Although effective, optical microstructures have been incorporated directly onto the surface of corrective lenses to date. The optical microstructures may be engraved, etched, or embossed directly onto either the convex surface of the corrective lens (e.g., the surface of the lens opposite the surface adjacent to the wearer's eye) or the concave surface of the corrective lens (e.g., the surface of the lens adjacent to the wearer's eye). In one example, this configuration may lead to scratches or other damage to the optical microstructures as a result of daily use. Furthermore, building optical microstructures directly onto the lens surface may require a unique design for each lens substrate material, since each design of the optical microstructure relies on the change in refractive index between the optical microstructure and the surrounding medium, and every lens substrate material requires a unique set of optical designs. Thus, each lens substrate material may require a unique optical microstructure architecture and configuration.
[0021] In addition to the above, casting a thermoset lens with optical microstructures on its surface presents technical challenges when integrated into an optical lens. For example, the optical microstructures or microlenses undergo different amounts of shrinkage when different monomers are used. In addition, high aspect ratios between the lens center and the lens edge may undergo different amounts of shrinkage in the same monomer. This is especially problematic for optical microstructures with very small dimensions. Such issues will affect the microlens design in the final product and may require multiple iterations of mold design changes to arrive at the final desired design. Furthermore, having microlenses on the lens surface exposes the microlenses to modifications by hard coatings, which must also be considered when designing and realizing the final design product.
[0022] According to one embodiment, the present disclosure provides an ophthalmic lens having an encapsulated optical microstructure that retains its structure after casting and hard coating. It includes a functional wafer (i.e., a first layer) having an optical microstructure on its surface. The functional wafer, which may be a thermoplastic resin, does not change shape during the polymerization cycle of a thermosetting monomer that contacts the surface of the functional wafer having the optical microstructure thereon. Furthermore, such encapsulation of the optical microstructure by the thermosetting monomer avoids the challenges presented by hard coating.
[0023] In one embodiment, the present disclosure provides for this purpose a microstructured thermoplastic wafer with a glass transition temperature higher than that of the thermosetting material by injection molding, roll-to-roll hot embossing, or film and / or laminate, which can be placed in the forming chamber cavity for casting against the inner surface of the forming chamber mold, or can be used as a mold in the forming chamber (e.g., against the front mold or as the mold that will be held after removal of the back mold). When the thermosetting monomer is introduced into the forming chamber cavity, the thermoplastic wafer can be oriented so that at least the surface of the thermoplastic wafer with the optical microstructure is exposed (alternatively, the second layer can be thermoplastic), so that the thermoplastic wafer comes into contact with the thermosetting monomer (i.e., the second layer). In this way, the optical microstructure can be encapsulated in the final optical lens design. In one example, both sides of the thermoplastic wafer can be exposed to the thermosetting monomer, whereby the thermoplastic wafer is sandwiched between the thermosetting monomer. After casting and polymerization of the thermoset monomer, the casting mold can be removed and the resulting dual-material lens (thermoset / thermoplastic) has encapsulated microstructures that have the exact same design as those used in the thermoplastic wafer and do not change shape due to different amounts of monomer shrinkage during casting or as a result of further lens processing.
[0024] Since the microlens has a refractive power, i.e., ΔRI=RI Wafer -RI Lens ≒0, the refractive index (RI Wafer and R.I. first layer The refractive index (RI) of a lens is Lens and R.I. second layer (also called
[0025] Typically, the refractive index (RI) of the thermoplastic resin wafer Wafer and R.I. first layer Also called the refractive index (RI) of the lensLens and R.I. second layer (also referred to as ) is greater than 0.01, preferably greater than 0.04, and typically greater than 0.05, for example 0.07.
[0026] According to the present invention, the refractive index (RI) of the thermoplastic resin wafer Wafer ) and the refractive index of the lens (RI Lens ) is greater than 0.01" includes the following values and / or any intervals between the following values (including the boundaries): 0.01; 0.02; 0.03; 0.04; 0.05; 0.06; 0.07; 0.08; 0.09; 0.1; 0.2; 0.3 etc.
[0027] In one embodiment, the thermoplastic wafer may be a Durabio™ microstructured wafer with a thermoset monomer (i.e., a thermoset lens) disposed between or on the MR8 lens. The refractive index difference (ΔRI) between the thermoset monomer and the thermoplastic wafer may be about 0.1.
[0028] In another example, the thermoplastic wafer may be a polycarbonate microstructured wafer with a thermoset monomer (i.e., a thermoset lens) disposed between or on the surface of the MR7 lens. The (ΔRI) between the thermoset monomer and the thermoplastic wafer may be about 0.07.
[0029] In one embodiment, for myopia control, the optical power of the optical microstructures can be positive to provide peripheral defocus that slows myopia progression. If ΔRI>0, then the optical microstructures on the wafer can be convex, e.g., as in Figures 4A and 4B, with positive optical power. If ΔRI<0, then the optical microstructures on the wafer can be concave, e.g., as in Figures 5A and 5B, with positive optical power.
[0030] In one embodiment, the optical power of the optical microstructures is also a function of the radius, cylindricity, and / or asphericity that ultimately define the shape of each optical microstructure. Therefore, maintaining the shape integrity of the optical microstructures under the high temperature and pressure of injection overmolding helps to maintain the optical design. It is also necessary to ensure that the interface between the wafer and the lens is clear and well-defined to have high optical fidelity. In addition, the bond between the wafer and the lens can be strong enough to survive the hard multi-coating (HMC) and Rx surfacing, edging, and mounting processes.
[0031] In one embodiment, the thermal resistance of the wafer material can be made greater than that of the lens material to withstand the high temperatures and pressures of injection overmolding or the high curing temperatures of casting thermoset resins to maintain the geometric integrity of the optical microstructures. For plastic materials, the thermal resistance can be determined by the glass transition temperature (T g ) can be characterized by T g The higher the temperature, the higher the heat resistance. Therefore, in order to prevent the microlenses from deforming, the glass transition temperature (T g,Wafer And, T g First layer The glass transition temperature (T g,Lens And, T g Second layer Furthermore, T g,Wafer is T g,Lens At least 5°C higher than T g,Wafer >T g,Lens +5°C is highly desirable.
[0032] According to the present invention, "T g,Wafer and Tg Lens"at least 5°C between" includes the following values and / or any intervals included between the following values (including the boundaries): 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 35, 40, 45, 50, 55, 60, 65, 66, 67, 68, 69, 70, etc. According to one embodiment, T g,Wafer is T g,Lens is at least 8°C, preferably at least 10°C, especially at least 15°C, and typically at least 20°C.
[0033] In one embodiment, to achieve a transparent and well-defined interface and obtain strong bonding, the wafer material and the lens material can contain the same or similar functional groups in their repeating chemical structural units to have the necessary miscibility. Transparent thermoplastics with ester groups -OC(=O) including carbonate ester -OC(=O)-O- are miscible with each other. Some examples include polycarbonate, poly(methyl methacrylate) (PMMA), and copolyesters, among others. Transparent thermoplastics with amide groups -C(=O)-N= are miscible with each other. Some examples include polyamides and polyurethanes.
[0034] According to one embodiment, the present disclosure provides the ability to create heat-cured lenses with encapsulated microstructures, where the heat-cured lenses can be coated with any coating, where the coating does not affect the design of the microstructure, and the encapsulation of the microstructure enhances the mechanical properties (e.g., impact resistance) of the lens.
[0035] In one embodiment, the present disclosure avoids the need to create a microstructured glass mold for casting. Furthermore, when a thermoplastic wafer is used as the mold component, the present disclosure provides a means to use UV polymerization through a transparent mold.
[0036] According to one embodiment, the present disclosure provides an opportunity to introduce light filters into an ophthalmic lens via a thermoplastic wafer.
[0037] According to one embodiment, the present disclosure allows for a reduction in the unit cost of a microstructured thermoplastic wafer (eg, a polycarbonate (PC) wafer) with an increased amount of heat cured lenses.
[0038] Referring now to the drawings, FIG. 1 provides a schematic diagram of a forming chamber or molding device for incorporating thermoplastic wafers into optical lenses.
[0039] The molding device can include a first molding surface 145a, a second molding surface 145b, a concave molding insert 141, and a convex molding insert 142. Each of the first molding surface 145a and the second molding surface 145b can include a hollow portion into which the concave molding insert 141 and the convex molding insert 142 can be removably disposed. In one embodiment, either or both of the concave molding insert 141 and the convex molding insert 142 can be replaced with a thermoplastic wafer, which forms a cavity into which a thermosetting monomer can be introduced.
[0040] Assuming the mold inserts are held as shown in FIG. 1, a first mold surface 145a including a concave mold insert 141 can be configured to mate with a second mold surface 145b including a convex mold insert 142. When mated, the concave mold insert 141 and the convex mold insert 142 can form a cavity 150 connected to a hollow line 160 formed by the mating of the first and second mold surfaces 145a, 145b. The hollow line 160 can be configured to receive a polymer or prepolymer, for example, via a screw feeder or similar device. In an embodiment, a wafer 102 (such as, but not limited to, a thermoplastic or thermoset wafer) having optical microstructures 103 can be placed in the cavity 150. In FIG. 1 , the optical microstructure 103 is on a first surface 106, i.e., concave surface 106, of the wafer 102, which has a second surface, i.e., convex surface 107, opposite the concave surface 106. During formation, once the wafer 102 is placed in the cavity 150, a second layer (e.g., but not limited to, a thermosetting layer) can be formed by flowing a thermosetting monomer into the cavity 150 via the hollow line 160. It can be understood that a thermoplastic resin layer for the second layer can be formed instead (instead of a thermosetting layer for the second layer) by flowing a thermoplastic material into the cavity 150. Notably, the glass transition temperature of the wafer 102 is greater than the corresponding glass transition temperature of the thermosetting layer, thus allowing the thermosetting monomer to flow and harden without destroying the structure of the wafer 102. Depending on the placement of wafer 102 (e.g., against convex mold insert 142, against concave mold insert 141, and spaced between and from concave mold insert 141 and convex mold insert 142), it may be possible for the thermosetting monomer to fill the remaining space of cavity 150. In one embodiment, the thermosetting monomer may be flowed such that it only contacts concave surface 106 of wafer 102. Once cured, the optical microstructures 103 on concave surface 106 of wafer 102 may then be encapsulated by the thermosetting layer.
[0041] In one embodiment, the curvature of the concave mold insert 141 and the curvature of the convex mold insert 142 contribute to the lens power of the resulting lens. In one embodiment, for a semi-finished lens, the curvature along the concave side of the optical lens is fixed, and the convex side of the optical lens may be altered after molding, for example, via grinding and polishing. It is noted that multiple lines for receiving polymer can be connected together so that one injection of polymer from a source can fill multiple molding devices with a single injection, allowing for parallel production of multiple lenses.
[0042] In one embodiment, prior to being placed in the molding device, the wafer 102 may be thermoformed into a spherical dome shape, for example, by a thermoforming machine. It may be appreciated that known devices and methods may be used to thermoform the wafer 102. For example, a LEMA manufacturing machine may be used that progressively increases the curvature of a flat wafer under the application of heat.
[0043] In one embodiment, the optical lens may comprise a thermoset polyurethane, an allyl diglycol carbonate, a polythiourethane, an episulfur polymer, an epoxy, a poly(meth)acrylate, a polythiomethacrylate, or a combination thereof, typically a poly(meth)acrylate.
[0044] In one embodiment, the wafer 102 may be one of a variety of suitable substrates including (meth)acrylic (co)polymers, particularly methyl PMMA, polyvinyl butyral (PVB), polycarbonate, thermoplastic polyurethane (TPU), thermoplastic copolymers of ethylene and vinyl acetate, polyesters such as polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), polycarbonate and polyester copolymers, cycloolefin copolymers such as ethylene and norbornene or ethylene and cyclopentadiene copolymers, and combinations thereof. As used herein, "(co)polymer" refers to a copolymer or polymer. A (meth)acrylate is an acrylate or methacrylate.
[0045] According to one embodiment, the wafer 102 is made of polycarbonate (PC).
[0046] According to the present invention, "polycarbonate" (PC) refers to homopolycarbonates, copolycarbonates and block copolycarbonates. Polycarbonates may be aromatic or non-aromatic. Aromatic polycarbonates are commercially available, for example, from Sabic under the trade name Lexan™, from Teijin Limited under the trade name Panlite™, from Covestro under the trade name Makrolon™, and from Mitsubishi Engineering Plastics Corporation under the trade name Iupilon™. Non-aromatic polycarbonates are commercially available, for example, from Mitsubishi Chemical Corporation under the trade name Durabio™.
[0047] With that in mind, and now with reference to FIG. 2, a method of forming an ophthalmic lens according to an exemplary embodiment of the present disclosure will be described.
[0048] FIG. 2 provides an illustration of a method 200 of forming an ophthalmic lens having optical microstructures encapsulated therein.
[0049] In step 205 of method 200, a first layer (e.g., a thermoplastic or thermosetting layer) may be provided along with a cavity of a forming chamber, for example as described with reference to FIG. 1. The first layer may have a first surface and a second surface, the first surface having an optical microstructure formed thereon and the second surface is opposite the first surface. The first layer may be disposed within the cavity of the forming chamber based on the characteristics of the desired optical lens to be formed. For example, with general reference to FIGS. 3A and 3B, the desired optical lens may have a second layer (e.g., a thermoplastic or thermosetting layer) contacting only the first surface of the first layer. Thus, the first layer may be provided within the cavity of the forming chamber against a concave mold insert. In another example, with general reference to FIGS. 3C and 3D, the desired optical lens may have a second layer (e.g., a thermoplastic or thermosetting layer) contacting both the first surface of the first layer and the second surface of the first layer. Thus, the first layer may be disposed within the cavity of the forming chamber between and spaced from the concave and convex mold inserts.
[0050] Optionally, an adhesion promoting layer may be provided on the first surface of the first layer to "prime" the first layer for bonding to the thermosetting monomer or thermoplastic material of the second layer. Such modifications are described in more detail with reference to subsequent figures.
[0051] Alternatively, the optical microstructures may be formed on a second surface of the first layer, upon which the second layer can be formed.
[0052] In one embodiment, each of the optical microstructures on the first surface of the first layer may have a dimensional height, a dimensional width, and may be separated from an adjacent one of the optical microstructures by a predetermined distance that defines an area between the optical microstructures. Each area between the optical microstructures may have a dimensional height that defines a distance between the first surface of the first layer and the base of each of the optical microstructures. Each of the optical microstructures may have a variety of shapes, including hemispherical, rectangular, cylindrical, pyramidal, circular, elliptical, and prismatic, among others, as required by visual requirements. The curvature of each optical microstructure may be linear, curved, or a combination thereof.
[0053] In one embodiment, the optical microstructures may be formed by one of several methods. In one example, a nickel-platinum plated shim or a nickel-silicon plated shim may be used to emboss a given optical microstructure architecture and design onto the first surface of the first layer. In another example, energy-assisted imprinting may be used to stamp the first surface of the first layer to provide the optical microstructures thereon. To solidify the optical microstructures on the first surface of the first layer, imprinting may be assisted by stamping a thin coating layer of reactive material (e.g., energy curable material, reactive, crosslinkable, etc.) or phase change material (e.g., liquid-crystalline solid, liquid crystal material). For example, imprinting may use an ultraviolet process, in which a thin coating layer of ultraviolet curable material is applied to the first surface of the first layer, a replica stamp is used to generate an embossed pattern of the optical microstructures, and then cured with ultraviolet light to solidify the pattern of the optical microstructures on the first surface of the first layer. Although an ultraviolet process may be used, in one embodiment, thermal processes as well as electron beam processes may also be used.
[0054] In one embodiment, photolithography and / or direct write additive manufacturing can also be used to generate optical microstructures in the first surface of the thermoplastic resin.
[0055] In one embodiment, photolithography and / or direct write additive manufacturing can also be used to generate optical microstructures in the first surface of the thermoset resin.
[0056] In one embodiment, injection molding can also be used to form a thermoplastic layer having optical microstructures in a first surface of the thermoplastic.
[0057] In one embodiment, thermoset casting may also be used to form a thermoset layer having optical microstructures within a first surface of the thermoset resin.
[0058] In one embodiment, the process described above can produce a negative optical microstructure (i.e., a negative pattern), which can be of the same material as the first layer or a different material. A roll or flat stamp with a mirror image (i.e., a positive pattern) of the embossed pattern of the optical microstructures can be used as a template to form a pattern of the fluid UV-curable material. UV curing of the material can follow to set the pattern.
[0059] In view of the above, it will be appreciated that the stamping technique can produce either concave or convex optical microstructures relative to the first surface of the first layer, based on the design of the template used during the stamping technique.
[0060] Returning to method 200, in step 205, after placing the first layer within the cavity of the forming chamber, a thermosetting material (for the second layer, which is a thermosetting layer) may be flowed into the cavity of the forming chamber and contact the first surface of the first layer. In one embodiment, the thermosetting material may be a thermosetting monomer. In step 215 of method 200, the thermosetting material is cured, thereby encapsulating the optical microstructures within the ophthalmic lens via the formed second layer (e.g., the thermosetting layer).
[0061] In an optional embodiment, the method 200 includes depositing a protective layer on the exposed surface of the ophthalmic lens at step 220. For example, as in FIG. 3B, the exposed surface of the ophthalmic lens may be a second surface of a thermoplastic material. In another example, as in FIG. 3D, the exposed surface of the ophthalmic lens may be a surface of a second layer of a thermosetting material deposited on the second surface of the first layer. In one example, the protective layer may be a hard coating that provides certain abrasion and / or scratch resistance properties to the ophthalmic lens. The hard coating may be a Mithril hard coating (Essilor), specifically based on a hydrolyzate of γ-glycidoxypropyltrimethoxysilane (GLYMO) and dimethyldiethoxysilane (DIVIDES) with colloidal silica and aluminum acetylacetonate. Further discussion of the protective layer will be described in more detail with reference to the remaining figures.
[0062] An exemplary ophthalmic lens resulting from performance of method 200 will now be described with reference to Figures 3A-6B.
[0063] 3A, 4A and 5A, an ophthalmic lens 301 may include a thermoplastic layer 302 and a thermosetting layer 304. An optical microstructure 303 may be formed in / on a first surface 306 of the thermoplastic layer 302. As in FIG. 4A, the first surface 306 of the thermoplastic layer 302 may be treated such that the optical microstructure 303 thereon appears embossed on the first surface 306 of the thermoplastic layer 302. As can be seen, the optical microstructure 303 on the first surface 306 of the thermoplastic layer 302 is hemispherical and convex in shape. Now referring to FIG. 5A, the first surface 306 of the thermoplastic layer 302 may be treated such that the optical microstructure 303 thereon appears embossed on the first surface 306 of the thermoplastic layer 302. As can be seen, the optical microstructure 303 on the first surface 306 of the thermoplastic layer 302 is hemispherical and concave in shape.
[0064] In one embodiment, the thermosetting layer 304 may generally be made of a cross-linked material (e.g., a thermosetting material). In particular, the thermosetting layer 304 may be obtained by polymerization of an allyl derivative, such as an allyl carbonate, of a linear or branched aliphatic or aromatic polyhydric alcohol. This may further include diethylene glycol bis(allyl carbonate), isopropyl ene bisphenol-A bis(allyl carbonate), matrices based on poly(meth)acrylates and copolymers, polythio(meth)acrylates, thermosetting polyurethanes, polythiourethanes, polyepoxides, polyepisulfides, as well as copolymers and blends thereof. In one embodiment, the thermosetting layer 304 may be a (co)polymerized bisallyl carbonate of diethylene glycol, such as an Orma® (Essilor) matrix, for example, commercially available as CR-39® by PPG Industries.
[0065] According to one embodiment, the thermoplastic layer 302 (ie, the first layer / wafer) may be polycarbonate (PC) or poly(meth)acrylate (PMMA).
[0066] For example, suitable materials for forming the first thermoplastic layer 302 (ie, the first layer) have the following Tg:
[0067] [Table 1]
[0068] Now referring to FIG. 3B, the Ophthalmic Lens 301 of FIG. 3A may be further modified to include a protective layer 308 on the second surface 307 of the thermoplastic layer 302. The protective layer 308 may be at least one of a urethane coating, an acrylic coating, an epoxy coating, a scratch-resistant coating, an anti-reflective coating, a photochromic coating, an anti-soiling coating, an anti-fog coating, a tinted coating, a self-repelling coating, a water-repellent coating, an anti-static coating, an anti-UV coating, and a blue light cut coating, among others. For example, the protective layer 308 may be a hard coating that provides certain abrasion and / or scratch resistance properties to the Ophthalmic Lens 301. An exposed surface 318 of the protective layer 308 may face the external environment of the Ophthalmic Lens 301. When the protective layer 308 is a hard coating, the hard coating may be a Mithril hard coating (Essilor). Specifically, the hard coating may be based on a hydrolyzate of γ-glycidoxypropyltrimethoxysilane (GLYMO) and dimethyldiethoxysilane (DIVIDES) with colloidal silica and aluminum acetylacetonate. In one embodiment, the protective layer 308 may be a Mithril hard coating and may have a thickness of 3.5 μm.
[0069] In one embodiment, the Mithril hard coating may have a refractive index of about 1.5. In a particular example, the Mithril hard coating may have a refractive index of 1.6. The Mithril hard coating may have a thickness of 3 μm to 6 μm and may be applied to the Ophthalmic Lens 301 by dip coating or the like.
[0070] 3C, 4B and 5B, an ophthalmic lens 301 may include a thermoplastic layer 302, a first thermosetting layer 304, and a second thermosetting layer 304'. The first thermosetting layer 304 may be formed on the first surface 306 of the thermoplastic layer 302 as in the previous embodiment. Furthermore, the second thermosetting layer 304' may be formed on the second surface 307 of the thermoplastic layer 302. An optical microstructure 303 may be formed in / on the first surface 306 of the thermoplastic layer 302. As in FIG. 4B, the first surface 306 of the thermoplastic layer 302 may be treated such that the optical microstructure 303 thereon appears embossed on the first surface 306 of the thermoplastic layer 302. As can be seen, the optical microstructure 303 on the first surface 306 of the thermoplastic layer 302 is hemispherical and convex in shape. 5B, the first surface 306 of the thermoplastic layer 302 may be treated such that the optical microstructures 303 thereon appear embossed onto the first surface 306 of the thermoplastic layer 302. As can be seen, the optical microstructures 303 on the first surface 306 of the thermoplastic layer 302 are hemispherical and concave in shape.
[0071] In one embodiment, the first thermosetting layer 304 and the second thermosetting layer 304' may generally be made of cross-linked materials (e.g., thermosetting materials). In particular, the first thermosetting layer 304 and the second thermosetting layer 304' may be obtained by polymerization of allyl derivatives, such as allyl carbonates, of linear or branched aliphatic or aromatic polyhydric alcohols. This may further include diethylene glycol bis(allyl carbonate), isopropyl ene bisphenol-A bis(allyl carbonate), matrices based on poly(meth)acrylates and copolymers, polythio(meth)acrylates, thermosetting polyurethanes, polythiourethanes, polyepoxides, polyepisulfides, and copolymers and blends thereof. In one embodiment, the thermosetting layer 304 may be a (co)polymerized bisallyl carbonate of diethylene glycol, such as an Orma® (Essilor) substrate, for example, commercially available as CR-39® by PPG Industries. It will be understood that the specific materials described for the thermosetting layer 302, the first thermosetting layer 304, and the second thermosetting layer 304' may be replaced or substituted with other materials, for example, the thermosetting layer 302 may be the thermosetting layer 302, or the first thermosetting layer 304 may be the first thermosetting layer 304, or the second thermosetting layer 304' may be the second thermosetting layer 304', among other combinations.
[0072] Now referring to Figure 3D, the Ophthalmic Lens 301 of Figure 3C may be further modified to include a protective layer 308 on the surface 314 of the second thermosetting layer 304. The protective layer 308 may be at least one of a urethane coating, an acrylic coating, an epoxy coating, a scratch-resistant coating, an anti-reflective coating, a photochromic coating, an anti-soiling coating, an anti-fog coating, a tinted coating, a self-repelling coating, a water-repellent coating, an anti-static coating, an anti-UV coating, and a blue light cut coating, among others. For example, the protective layer 308 may be a hard coating that provides certain abrasion and / or scratch-resistant properties to the Ophthalmic Lens 301. An exposed surface 318 of the protective layer 308 may face the external environment of the Ophthalmic Lens 301.
[0073] When the protective layer 308 is a hard coating, the hard coating may be a Mithril hard coating (Essilor). Specifically, the hard coating may be based on a hydrolyzate of γ-glycidoxypropyltrimethoxysilane (GLYMO) and dimethyldiethoxysilane (DIVIDES) with colloidal silica and aluminum acetylacetonate. In one embodiment, the protective layer 308 may be a Mithril hard coating and may have a thickness of 3.5 μm.
[0074] In one embodiment, the Mithril hard coating may have a refractive index of about 1.5. In a particular example, the Mithril hard coating may have a refractive index of 1.6. The Mithril hard coating may have a thickness of 3 μm to 6 μm and may be applied to the Ophthalmic Lens 301 by dip coating or the like.
[0075] Returning now to Figures 6A and 6B, the method 200 can be improved by the addition of an adhesion-promoting or bonding layer that strengthens the interface between the layers of the Ophthalmic Lens. Accordingly, Figures 6A and 6B illustrate an Ophthalmic Lens 601 formed using an adhesion-promoting layer.
[0076] Referring first to Figure 6A, similar to that shown in Figures 3A, 4A, and 5A, an Ophthalmic Lens 601 includes a thermosetting layer 604 and a thermoplastic layer 602, the thermoplastic layer 602 having optical microstructures 603 on a first surface 606 thereof. Additionally, the Ophthalmic Lens 601 may include an adhesion promoting layer 609 disposed on the first surface 606 of the thermoplastic layer 602. The adhesion promoting layer 609 may or may not be in contact with the optical structures 603 on the first surface 606 of the thermoplastic layer 602. In one embodiment, the adhesion promoting layer 609 may be an adhesive system such as a pressure sensitive adhesive or a hot melt adhesive, a corona-mediated surface activation method, or a plasma- or ozone-mediated surface activation method, among others. In one embodiment, the adhesion promoting layer 609 may be a primer coating comprising an acrylic monomer or a mixture of an acrylic monomer and an alkoxysilane having a reactive group selected from the group including allyl, vinyl, acrylic, thiol, isocyanate, epoxy, and amine, and a photoactive catalyst including a cationic photoinitiator such as UVI-6976, and a free radical photoinitiator such as DAROCUR 1173.
[0077] Secondly, referring to FIG. 6B, similar to that shown in FIG. 3C, FIG. 4B, and FIG. 5B, an ophthalmic lens 601 includes a first thermosetting layer 604, a second thermosetting layer 604', and a thermoplastic layer 602, the thermoplastic layer 602 having optical microstructures 603 on its first surface 606. As in FIG. 6A, the ophthalmic lens 601 may further include an adhesion promoting layer 609 disposed on the first surface 606 of the thermoplastic layer 602 and on the second surface 607 of the thermoplastic layer 602. The adhesion promoting layer 609 may be configured to contact each of the first thermosetting layer 604 and the second thermosetting layer 604'. The adhesion promoting layer between the first thermosetting layer 604 and the thermoplastic layer 602 may or may not contact the optical microstructures 603 on the first surface 606 of the thermoplastic layer 602. In one example, the adhesion promoting layer 609 may be an adhesive system such as a pressure sensitive adhesive or a hot melt adhesive, a corona-based surface activation method, or a plasma-based or ozone-based surface activation method, among others. In one embodiment, the thermoplastic layer 602 may instead be another thermosetting layer.
[0078] Again, it will be understood that the particular materials described for the thermoplastic layer 602, the first thermosetting layer 604, and the second thermosetting layer 604' may be exchanged or substituted with other materials, for example, the thermoplastic layer 602 may be the thermosetting layer 602, or the first thermosetting layer 604 may be the first thermoplastic layer 604, or the second thermosetting layer 604' may be the second thermoplastic layer 604', among other combinations.
[0079] FIG. 8 provides an illustration of a method 800 for forming an ophthalmic lens having optical microstructures encapsulated therein, according to another embodiment, where instead of a thermosetting layer and a thermoplastic layer having different glass transition temperatures, two thermoplastic layers having different glass transition temperatures are used.
[0080] In step 805 of method 800, a first thermoplastic layer may be provided in a cavity of a forming chamber, for example as described with reference to FIG. 1. The thermoplastic layer may have optical microstructures formed on a first surface of the first thermoplastic layer. In step 810 of method 800, a thermoplastic material may be flowed into the cavity of the forming chamber and contact a surface of the first thermoplastic material to form a second thermoplastic layer. In step 815, the second thermoplastic material is cooled to form a lens encapsulating the microstructures. If the material flowed into the cavity of the forming chamber is a second thermoplastic, the glass transition temperature of the first thermoplastic layer is higher than the glass transition temperature of the second thermoplastic layer, and the first thermoplastic layer and the second thermoplastic layer have miscible functional groups. In one example, the first thermoplastic layer may be bisphenol-A polycarbonate with a glass transition temperature of 147° C. and the second thermoplastic layer of PMMA has a glass transition temperature of 120° C. and has miscible functional groups.
[0081] Ophthalmic lenses made according to the above process will now be described. Exemplary lenses were made and evaluated according to standard techniques. EXAMPLES
[0082] The experiment involves casting a thermoset material (MR 7 with an e-line refractive index of 1.665) with a thermoplastic wafer (PC with an e-line refractive index of 1.591). The materials used are as in Table 1.
[0083] [Table 2]
[0084] Initial testing was performed with a PC semi-finished lens (base 3.25) carrying optical microstructures or microlenses patterned on the backside. The semi-finished lens was thinned by surfacing to obtain a suitable thickness for use as a wafer. After surfacing, the wafer was cleaned with isopropyl alcohol to remove dust and contamination. The wafer was then mated with a standard mineral back mold (80 mm) to taper at the desired center thickness. In other words, referring to FIG. 1, the wafer forms a concave mold insert 141 and the standard mineral back mold forms a convex insert 142, with the space between them determining the desired center thickness. The standard mineral back mold may be a standard MR 7 mold.
[0085] In this example, the thermosetting material is a monomer blend. The monomer mix can be prepared by weighing and mixing the ingredients in Table 1. Mixing can include application of nitrogen gas under a vacuum connection. Mixing can include first adding monomer MR 7 A, followed by DMC, UV 701, and Zelec UN. The mixture can be mixed under vacuum until homogenous. The mixer can then be cooled. Following cooling, MR7 B and the bluing agent can be added and mixed under vacuum.
[0086] The previously prepared mold (i.e., wafer and standard mineral back mold) can be filled with the prepared thermosetting monomer using a cleaned syringe, and polymerization can be achieved in a conditioned microwave oven. For example, the polymerization reaction can be carried out in a microwave oven according to the following cycle: (1) about 10-20°C for 12 hours, (2) a gradual increase in temperature from 20°C to 120°C at a rate of about 5°C / h to 25°C / h over 7 hours, (3) about 100-120°C for 4 hours. After polymerization, the assembly can be removed from the oven and the standard mineral back mold can be disassembled. The thermoplastic resin layer or the concave mold insert 141 is now part of the final lens.
[0087] After disassembly, the ophthalmic lenses and the convex mold inserts were cleaned. The ophthalmic lenses were immersed and sonicated in a surfactant solution, rinsed, and dried. The convex mold inserts were cleaned in hot concentrated sulfuric acid and rinsed with water.
[0088] The formed ophthalmic lenses are then evaluated according to conventional testing techniques. For example, measurements include percent (%) transmittance, measurements of light passing through the material, UV cutoff, measurements of the maximum wavelength at which transmittance is less than 1%, Yellowness Index (YI), colorimetric calculations from tristimulus values (X, Y, Z) (following ASTM D1003 standard), and optical properties including microlens power (e.g., central, global, peripheral), Rx power (e.g., sphere, cylinder, cylinder axis), lens geometric center, microlens network center, and Rx optical center. Such optical properties and other lens characteristics can be measured by software and hardware systems dedicated to such purposes.
[0089] The results of the ophthalmic lenses prepared according to the methods described herein are shown in Table 2. It can be seen that the values of each listed characteristic meet the established lens performance requirements. Most importantly, the global refractive power average of the microlenses measured with an imaging device (e.g., using an analytical tool from Essilor called Jarvis Clear-Reader) is consistent with the design goal shown in FIG. 7. According to the present invention, the "global average refractive power" measures the refractive power profile of the microlenses of the ophthalmic lens. According to the illustrated embodiment, the microlenses are arranged in concentric rings such as R01-R11 (pattern of optical microstructures), with the microlenses located within one ring (e.g., R01) forming a set of microlenses. In this case, the set of microlenses considered to average the global refractive power corresponds to all the microlenses that are in the same "ring".
[0090] [Table 3]
[0091] As can be seen from the above, the methods of the present disclosure allow for the production of thermoset lenses with similar myopia control and other features to those developed for thermoplastics, a development important for consumers to have access to innovative material independent products.
[0092] Example 1 (Invention) - The experiment involves overmolding a thermoplastic wafer (PC) with a thermoplastic material (PMMA).
[0093] Sabic Lexan™ OQ3820, a bisphenol-A polycarbonate with a refractive index of 1.591 and a glass transition temperature of about 147° C., was used to injection mold a φ76 mm CT 1.1 mm flat PC wafer with convex optical microstructures (microlenses) on the concave surface. With reference to FIG. 1 , a wafer 102 (e.g., but not limited to, a thermoplastic or thermoset wafer) was placed against the concave surface of a standard chrome-plated concave mold insert 141, and a standard chrome-plated steel insert formed the convex mold insert 142, with the space between them determining the desired thickness. Encapsulation of the microlenses was performed using Roehm America ACRYLITE™ hw55 PMMA with a refractive index of 1.513 and a glass transition temperature of 120° C. The melt and mold temperatures for the overmolding process were set at 240° C. and 100° C., respectively. Results The microlens refractive power of the PC / PMMA composite lens was measured using an imaging device.
[0094] FIG. 9 is an optical image of a PC / PMMA composite lens according to one embodiment of the present disclosure. As can be seen from FIG. 9, the image of the composite lens shows a very well-defined boundary between the microlenses and the base lens, and the overall refractive power average of the microlenses in each ring is as expected. This therefore suggests that the shape integrity of the microlenses is preserved. Furthermore, the PC / PMMA composite lens was passed through the HMC and Rx surfacing / edging process. As a result, the two layers did not separate. This indicates that the bond between PC and PMMA is strong. This result also proves that PC and PMMA are miscible due to the similarity of the ester groups in their repeating chemical structure units.
[0095] Example 2 (Comparative) - A φ76 mm CT 1.1 mm planar ACRYLITE® hw55 PMMA wafer (Tg of 120° C.) with concave microlenses on the concave surface was fabricated by injection molding. After the process described in Example 1, encapsulation of the microlenses was performed using Lexan® OQ3820 PC (Tg of 147° C.). The melt and mold temperatures for the overmolding process were set at 270° C. and 110° C., respectively.
[0096] FIG. 10 is an optical image of a PC / PMMA composite lens as a comparative example. As can be seen from FIG. 10, unlike the PC / PMMA case in Example 1, the image of the composite lens showed a blurred boundary between the microlenses and the base lens. The overall refractive power average of the microlenses in each ring was not measurable. This result suggests that the microlenses were deformed and that interdiffusion occurred at the PMMA / PC interface. Nevertheless, the PC / PMMA composite lens passed the Rx surfacing / edging process without delamination. This indicates that the bond between PMMA and PC is strong due to the similar ester groups in their repeating chemical structure units.
[0097] Example 3 (Invention) - The experiment involved overmolding a thermoplastic wafer (PC) with a thermoplastic material (Durabio).
[0098] Sabic Lexan™ OQ3820, a bisphenol-A polycarbonate with an e-line refractive index of 1.591 and a glass transition temperature of about 147° C., was used to injection mold a φ76 mm CT 1.1 mm planar PC wafer with convex microlenses. Referring to FIG. 1, a wafer 102 (such as, but not limited to, a thermoplastic or thermoset wafer) was placed against the concave surface of a standard chrome-plated concave mold insert 141, and a standard chrome-plated steel insert formed the convex mold insert 142, with the space between them determining the desired thickness. Encapsulation of the microlenses was performed by placing Mitsubishi Chemical Corporation's DURABIO™ D7340R, a bio-based isosorbide polycarbonate with a refractive index of 1.507 and a glass transition temperature of 125° C., into the mold. The melt and mold temperatures for the injection overmolding process were set at 240° C. and 100° C., respectively.
[0099] 11A is an optical image of a PC / Durabio composite lens, according to one embodiment of the present disclosure. As can be seen in FIG 11A, the image of the composite lens shows very well-defined boundaries between the microlenses.
[0100] FIG. 11B is a graph of the global refractive power average of the microlenses in each ring of an ophthalmic lens according to an embodiment of the present disclosure. In an embodiment, the microlens refractive power of the resulting PC / Durabio composite lenses was measured using an imaging device. The global refractive power average of the microlenses is consistent with the design goal shown in FIG. 11B. Furthermore, the PC / Durabio composite lenses passed through the HMC and Rx surfacing / edging processes without delamination, indicating strong bonding between PC and Durabio. This result also proves that PC and Durabio are miscible due to the similarity of carbonate ester groups in their repeating chemical structure units.
[0101] Example 4 (Comparative) - A 76 mm CT 1.1 mm planar DURABIO™ D7340R wafer (Tg of 125° C.) with concave microlenses on the concave surface was fabricated by injection molding. After the process described in Example 3, encapsulation of the microlenses was performed using Lexan® OQ3820 PC (Tg of 147° C.). The melt and mold temperatures for the injection overmolding process were set at 270° C. and 110° C., respectively.
[0102] FIG. 12 is a graph of the overall refractive power average of the microlenses in each ring. The microlens refractive power of the resulting Durabio / PC composite lenses was measured using an imaging device. As shown in FIG. 12, unlike the PC / Durabio case in Example 3, the overall refractive power average of the microlenses in each ring is below the expected result, suggesting that the microlenses were flattened during injection overmolding. Nevertheless, the Durabio / PC composite lenses passed the Rx surfacing / edging process without delamination. This indicates that the bond between Durabio and PC is strong due to the similar carbonate ester groups in their repeating chemical structure units.
[0103] Obviously, many modifications and variations are possible in light of the above teachings, and it is therefore to be understood that, within the scope of the appended claims, the embodiments of the present disclosure may be practiced other than as specifically described herein.
[0104] The embodiments of the present disclosure may be as shown in the parenthetical numbers below.
[0105] (1) An ophthalmic lens (601) comprising: a first layer (602), the first layer (602) having a microstructure (603) on a first surface (606) of the first layer (602), the microstructure (603) being formed in a certain pattern on the first surface (606) of the first layer (602), and the material of the first layer (602) being a thermoplastic material; and a second layer (604) formed on the first surface (606) of the first layer (602), the glass transition temperature of the first layer (602) being higher than the glass transition temperature of the second layer (604).
[0106] (2) An ophthalmic lens as described in (1), wherein the refractive index of the first layer (602) is different from the refractive index of the second layer (604).
[0107] (3) An ophthalmic lens according to either (1) or (2), wherein each microstructure of the microstructures (603) is a positive power lenslet.
[0108] (4) The ophthalmic lens according to any one of (1) to (3), wherein the material of the second layer (604) is a thermosetting material or a thermoplastic material.
[0109] (5) An ophthalmic lens according to any one of (1) to (4), further comprising an adhesion promoting layer (609) deposited on the first surface (606) of the first layer (602) and between the first layer (602) and the second layer (604).
[0110] (6) An ophthalmic lens according to any one of (1) to (5), further comprising a third layer (604') arranged on the second surface (607) of the first layer (602), the second surface (607) of the first layer (602) being opposite the first surface (606) of the first layer (602), the material of the second layer (604) being a thermosetting material, and the material of the third layer (604') being a thermosetting material.
[0111] (7) An ophthalmic lens according to any one of (1) to (6), further comprising an adhesion promoting layer (609) deposited on the second surface (607) of the first layer (602) and between the first layer (602) and the third layer (604').
[0112] (8) An ophthalmic lens according to any one of (1) to (7), further comprising at least one protective layer (308) deposited on at least one of the second surface (607) of the first layer (602) and the exposed surface of the second layer (604), wherein the second surface (607) of the first layer (602) is opposite the first surface (606) of the first layer (602), and the exposed surface of the second layer (604) is a surface of the second layer (604) that is not in contact with the first layer (602).
[0113] (9) A method of forming an ophthalmic lens having encapsulated lenslets, the method comprising: providing a first layer (602) in a cavity of a forming chamber, the first layer (602) having microstructures (603) on a first surface (606) of the first layer (602), the microstructures (603) on the first surface (606) of the first layer (602) being formed in a pattern, and a material of the first layer (602) being a thermoplastic material; flowing a second material into the cavity of the forming chamber and contacting the first surface (606) of the first layer (602); and setting the second material to form a second layer (604) on the first surface (606) of the first layer (602), wherein a glass transition temperature of the first layer (602) is higher than a glass transition temperature of the second layer (604).
[0114] (10) The method according to (9), wherein the refractive index of the first layer (602) is different from the refractive index of the second layer (604).
[0115] (11) The method according to either (9) or (10), wherein the material of the second layer (604) is a thermosetting material or a thermoplastic material.
[0116] (12) The method according to any one of (9) to (11), further comprising depositing an adhesion promotion layer (609) on the first surface (606) of the first layer (602) and between the first layer (602) and the second layer (604).
[0117] (13) The method according to any one of (9) to (12), further comprising depositing a protective layer (308) on at least one of the second surface (607) of the first layer (602) and the exposed surface of the second layer (604), wherein the second surface (607) of the first layer (602) is opposite the first surface (606) of the first layer (602) and the exposed surface of the second layer (604) is a surface of the second layer (604) that is not in contact with the first layer (602).
[0118] (14) The method of any one of (9) to (13), wherein the second material is a thermosetting material, and flowing the second material into the cavity of the forming chamber further comprises flowing the second material into the cavity of the forming chamber to contact a first surface (606) of the first layer (602) and a second surface (607) of the first layer (602), the second surface (607) of the first layer (602) being opposite the first surface (606) of the first layer (602), and setting the second material further comprises hardening the second material to form a second layer (604) on the first surface (606) of the first layer (602) and forming a third layer (604') on the second surface (607) of the first layer (602).
[0119] (15) The method according to any one of (9) to (14), wherein the first layer (602) and the second layer (604) have miscible functional groups.
[0120] (16) A method of forming an ophthalmic lens having encapsulated lenslets, the method comprising: providing a first layer (602) in a cavity of a forming chamber, the first layer (602) having microstructures (603) on a first surface (606) of the first layer (602), the microstructures (603) on the first surface (606) of the first layer (602) being formed in a pattern; flowing a thermoplastic material into the cavity of the forming chamber and contacting a surface of the first layer; and cooling the thermoplastic material to form a second layer on the surface of the first layer, wherein a glass transition temperature of the first layer is higher than a glass transition temperature of the second layer, and the first layer and the second layer have miscible functional groups.
[0121] (17) The method according to (16), wherein the refractive index of the first layer is different from the refractive index of the second layer.
[0122] (18) An ophthalmic lens according to any one of (1) to (8), wherein each microstructure is a convex lenslet or a concave lenslet.
[0123] (19) The ophthalmic lens according to any one of (1) to (8), wherein the protective layer (308) includes at least one of a urethane coating, an acrylic coating, an epoxy coating, a scratch-resistant coating, an anti-reflective coating, a photochromic coating, an anti-fouling coating, an anti-fog coating, a colored coating, a self-repellent coating, a water-repellent coating, an anti-static coating, an anti-UV coating, and a blue light cut coating.
[0124] (20) An ophthalmic lens (601), comprising: a first layer (602), the first layer (602) having a microstructure (603) on a first surface (606) of the first layer (602), the microstructure (603) on the first surface (606) of the first layer (602) being formed in a certain pattern, and a material of the first layer (602) being a thermosetting material; and a second layer (604) formed on the first surface (606) of the first layer (602), the glass transition temperature of the first layer (602) being higher than the glass transition temperature of the second layer (604).
[0125] Thus, the foregoing discussion merely discloses and describes exemplary embodiments of the present disclosure. As will be understood by those skilled in the art, the present disclosure may be embodied in other specific forms without departing from the spirit or basic characteristics of the present disclosure. Thus, the embodiments of the present disclosure are intended to be illustrative, but not limiting, of the scope of the present disclosure and other claims. The present disclosure defines in part the scope of the terms of the above claims, including all readily discernible variations of the teachings herein, so that the spirit of the present invention is not dedicated to the public. [Explanation of symbols]
[0126] 102 Wafer 103 Optical microstructure 106 First surface, concave 107 Second Surface, Convex 141 Concave molded insert 142 Convex molded insert 150 hollow 160 Hollow Line 301 Eye lenses 302 Thermoplastic resin layer 303 Optical microstructure 304 Thermosetting layer 306 First Surface 307 Second Surface 308 Protective layer 314 Surface 318 Exposed Surface 601 Eye lenses 602 First Layer 603 Optical microstructure 604 Second Layer 606 First Surface 607 Second Surface 609 Adhesion promotion layer
Claims
1. a first layer (302; 602), the first layer (302; 602) having a microstructure (303; 603) on a first surface (306; 606) of the first layer (302; 602), the microstructure (303; 603) on the first surface (306; 606) of the first layer (302; 602) being formed in a pattern, and the material of the first layer (302; 602) being a thermoplastic material; a second layer (304; 604) formed on the first surface (306; 606) of the first layer (302; 602), the glass transition temperature of the first layer (302; 602) being higher than the glass transition temperature of the second layer (304; 604); An ophthalmic lens comprising:
2. 2. An ophthalmic lens according to claim 1, wherein the refractive index of said first layer (302; 602) is different from the refractive index of said second layer (304; 604).
3. An ophthalmic lens according to claim 1 or 2, wherein each of said microstructures (303; 603) is a plus-power lenslet.
4. An ophthalmic lens according to any one of claims 1 to 3, wherein the material of the second layer (304; 604) is a thermosetting or thermoplastic material.
5. The ophthalmic lens of any one of claims 1 to 4, further comprising an adhesion promoting layer (609) deposited on the first surface (606) of the first layer (602) and between the first layer (602) and the second layer (604).
6. The ophthalmic lens of any one of claims 1 to 5, further comprising a third layer (604') arranged on a second surface (607) of the first layer (602), the second surface (607) of the first layer (602) being opposite the first surface (606) of the first layer (602), the material of the second layer (604) being a thermosetting material, and the material of the third layer (604') being a thermosetting material.
7. 7. The ophthalmic lens of claim 6, further comprising an adhesion promoting layer (609) deposited on the second surface (607) of the first layer (602) and between the first layer (602) and the third layer (604').
8. The ophthalmic lens of any one of claims 1 to 7, further comprising at least one protective layer (308) deposited on at least one of the second surface (307) of the first layer (302) and the exposed surface of the second layer (304), wherein the second surface (307) of the first layer (302) is opposite the first surface (306) of the first layer (302) and the exposed surface of the second layer (304) is a surface of the second layer (304) that is not in contact with the first layer (302).
9. A method for forming an ophthalmic lens (301; 601) having an encapsulated lenslet, said method comprising the steps of: Providing a first layer (302; 602) in a cavity (150) of a forming chamber, said first layer (302; 602) having a microstructure (303; 603) on a first surface (306; 606) of said first layer (302; 602), said microstructure (303; 603) on said first surface (306; 606) of said first layer (302; 602) being formed in a pattern, and a material of said first layer (302; 602) being a thermoplastic material; flowing a second material into the cavity (150) of the forming chamber and contacting the first surface (306; 606) of the first layer (302; 602); - setting said second material to form a second layer (304; 604) on said first surface (306; 606) of said first layer (302; 602); Including, A method, wherein the glass transition temperature of said first layer (302; 602) is higher than the glass transition temperature of said second layer (304; 604).
10. 10. The method of claim 9, wherein the refractive index of the first layer (302; 602) is different from the refractive index of the second layer (304; 604).
11. 11. The method according to claim 9 or 10, wherein the material of the second layer (304; 604) is a thermosetting or thermoplastic material.
12. The method according to any one of claims 9 to 11, further comprising depositing an adhesion promoting layer (609) on the first surface (606) of the first layer (602) and between the first layer (602) and the second layer (604).
13. 13. The method of any one of claims 9 to 12, further comprising the step of depositing a protective layer (308) on at least one of a second surface (307) of the first layer (302) and an exposed surface of the second layer (304), wherein the second surface (307) of the first layer (302) is opposite the first surface (306) of the first layer (302) and the exposed surface of the second layer (304) is a surface of the second layer (304) that is not in contact with the first layer (302).
14. the second material is a thermosetting material; Flowing the second material into the cavity (150) of the forming chamber further comprises flowing the second material into the cavity (150) of the forming chamber to contact the first surface (606) of the first layer (602) and a second surface (607) of the first layer (602), the second surface (607) of the first layer (602) being opposite the first surface (606) of the first layer (302; 602); 14. The method according to any one of claims 9 to 13, wherein the step of setting the second material further comprises: curing the second material to form the second layer (604) on the first surface (606) of the first layer (602); and forming a third layer (604') on the second surface (607) of the first layer (602).
15. The method of claim 14, wherein the first layer (302; 602) and the second layer (304; 604) have miscible functional groups.
Citation Information
Patent Citations