Rubber composition based on at least one compound having N-substituted imidazolidinone functionality

N-substituted imidazolidinone compounds improve the interaction between reinforcing fillers and diene elastomers, reducing hysteresis and enhancing rolling performance in tire rubber compositions.

JP7551733B2Active Publication Date: 2024-09-17MICHELIN & CO (CIE GEN DES ESTAB MICHELIN)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022507466
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-07
Filing Date
2020-08-06
Publication Date
2024-09-17
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

Tire manufacturers face challenges in reducing hysteresis in rubber compositions, which affects rolling resistance and fuel efficiency, despite existing modifications to diene elastomers using imidazolidinone functionality.

Method used

Incorporation of N-substituted imidazolidinone compounds into rubber compositions, which enhance the interaction between reinforcing fillers and diene elastomers through hydrogen bonding, leading to improved dispersion and reduced hysteresis.

Benefits of technology

The use of N-substituted imidazolidinone compounds results in a significant reduction of hysteresis, enhancing rolling performance and fuel efficiency in tire rubber compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551733000032
    Figure 0007551733000032
  • Figure 0007551733000007
    Figure 0007551733000007
  • Figure 0007551733000024
    Figure 0007551733000024
Patent Text Reader

Abstract

The present invention relates to a rubber composition based on at least one diene elastomer, at least one reinforcing filler, at least one chemical crosslinking system and, optionally, at least one compound of formula (I) pre-grafted to said diene elastomer: TIFF2022543634000051.tif5573In formula, A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear, or branched aliphatic hydrocarbon chains, which hydrocarbon chains are optionally substituted or interrupted by one or more heteroatoms; E is a divalent hydrocarbon group optionally containing one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom. The present invention relates to a rubber composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates in particular to a rubber composition that can be used to manufacture tire products, based on at least one diene elastomer, at least one reinforcing filler, at least one chemical crosslinking system, and at least one compound having an N-substituted imidazolidinone functional group, and also to a tire comprising such a composition. [Background technology]

[0002] In the industrial area of ​​objects made from rubber compositions, and in particular tires, mixtures of polymers containing reinforcing fillers are often used. There is a continuous search for ways to improve the dispersion of these reinforcing fillers in these polymers so that these compositions show better properties. The reason is that a good dispersion of these fillers in these polymers usually leads to a lower hysteresis and therefore a better rolling resistance when these rubber compositions are used in tires. On the other hand, improving the rolling resistance is a continuous challenge for tire manufacturers, since the need to save fuel and protect the environment has become a priority. In order to achieve the objective of reducing the hysteresis, many solutions have been proposed. In particular, reference may be made to the modification of the structure of the polymers, in particular diene elastomers, with modifiers at the end of the polymerization, with the aim of providing a good interaction between the polymers thus modified and the reinforcing fillers, be they carbon black or reinforcing inorganic fillers such as silica. Reference may be made, for example, to EP 0 778 311, which describes the use of diene polymers whose chain ends are functionalized with silanol groups. More recently, WO 2009 / 077837 describes elastomers functionalized with a silanol group at one chain end and an amino group at the other. These modified polymers are effective in reducing hysteresis. Summary of the Invention

[0003] However, tire manufacturers are still trying to reduce the hysteresis of rubber compositions. For this reason, research is being conducted on other reactions to modify polymers, especially diene elastomers, with the aim of obtaining rubber compositions with reduced hysteresis. In this respect, mention may be made of the use of compounds having nitrogen associative groups, which contain at least one unit that allows them to associate with each other via hydrogen bonds, to modify the polymers used in the rubber compositions. These modified polymers having unsubstituted imidazolidinone functional groups are described in WO 2019 / 007884. However, there is still a demand among tire manufacturers to further reduce the hysteresis of rubber compositions, which is the object of the present invention. Surprisingly, in the applicant's research, it was discovered that the use of compounds having N-substituted imidazolidinone functional groups in rubber compositions reduces the hysteresis of the composition compared to compositions containing compounds having unsubstituted imidazolidinone functional groups, and this object is achieved.

[0004] A subject of the present invention is a rubber composition based on at least one diene elastomer, at least one reinforcing filler, at least one chemical crosslinking system and, optionally, previously grafted to said diene elastomer, at least one compound of formula (I): [ka] During the ceremony, A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; E is a divalent hydrocarbon group, optionally containing one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom. Another subject of the invention relates to a semi-finished rubber product for tires, characterized in that it comprises a rubber composition as defined above. Another subject of the invention relates to at least one semi-finished product as defined above or to at least one rubber composition as defined above.

[0005] A first subject of the present invention relates to a rubber composition based on at least one diene elastomer, at least one reinforcing filler, at least one chemical crosslinking system and, optionally, previously grafted to said diene elastomer, at least one compound of formula (I): [ka] During the ceremony, A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; E is a divalent hydrocarbon group, optionally containing one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom.

[0006] The phrase "composition based on" should be understood to mean a composition comprising a mixture and / or in situ reaction products of the various components used, some of which can and / or are intended to react at least partially with one another during the various stages of the preparation of the composition, and thus the composition can be fully or partially crosslinked or non-crosslinked. In this specification, all percentages (%) refer to mass percentages (%), unless expressly indicated otherwise. Furthermore, any value interval expressed by the phrase "between a and b" refers to a range of values ​​greater than a and less than b (i.e. excluding the limits a and b), whereas any value interval expressed by the phrase "from a to b" refers to a range of values ​​from a to b (i.e. including the limits a and b). The compounds referred to in the description may be of fossil or biological origin. In the latter case, they may be partially or completely derived from biomass or may be obtained from renewable starting materials derived from biomass. The term "associative groups" is understood to mean groups capable of associating with one another in particular via hydrogen bonds, ionic bonds and / or hydrophobic bonds. According to a preferred embodiment of the invention, these are groups capable of associating with one another via hydrogen bonds. If the associative groups are capable of associating with one another via hydrogen bonds, each associative group preferably comprises at least one donor site and one site that is accepting for hydrogen bonds, so that two identical associative groups are self-complementary and can associate with the formation of at least two hydrogen bonds. The associative groups according to the invention can also associate with functional groups present on the filler, in particular on the reinforcing filler, and especially on reinforcing inorganic fillers such as silica, via hydrogen bonds, ionic bonds and / or hydrophobic bonds. The term "non-associative groups" is understood to mean groups that are not capable of associating with one another in particular via hydrogen bonds, ionic bonds and / or hydrophobic bonds. Preferentially, these are groups that are not capable of associating with one another via hydrogen bonds. These groups do not comprise a donor site and a site that is accepting for hydrogen bonds, so that none of these identical groups are self-complementary. They cannot associate together with the formation of at least two hydrogen bonds. Unless otherwise stated, the term "heteroatom" is understood to mean an atom selected from the group consisting of a sulfur atom, an oxygen atom, and a nitrogen atom. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Compounds of formula (I) As mentioned above, the rubber composition of the present invention is based on at least one compound of formula (I): [ka] During the ceremony, A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; E is a divalent hydrocarbon group, optionally containing one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom. A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms.

[0008] In the sense of the present invention, the term "arenediyl ring" is understood to mean a monocyclic or polycyclic aromatic hydrocarbon group derived from an arene by the removal of two hydrogen atoms. The arenediyl ring is therefore a divalent group. In the sense of the present invention, the term "monocyclic or polycyclic aromatic hydrocarbon group" is understood to mean one or more aromatic rings having a skeleton consisting of carbon atoms. That is, there are no heteroatoms in the skeleton of the ring. The arenediyl ring may be monocyclic, i.e. consisting of a single ring, or polycyclic, i.e. consisting of several fused aromatic hydrocarbon rings, such fused rings sharing at least two consecutive carbon atoms. These rings may be ortho-fused, or ortho-fused and peri-fused. Preferably, the arenediyl ring contains 6 to 14 carbon atoms. The arenediyl ring may be unsubstituted, partially or completely substituted. When the arenediyl ring is partially substituted, one or more hydrogen atoms (but not all atoms) are replaced by one or more, preferably saturated, linear or branched aliphatic hydrocarbon chains, which are optionally substituted with one or more heteroatoms. Said chains are also called substituents. When all hydrogen atoms are replaced by said chains, the arenediyl ring is fully substituted. The substituents of the arenediyl ring may be the same or different from each other. Preferably, when the arenediyl ring is substituted by one or more, preferably saturated, linear or branched aliphatic hydrocarbon chains, which are optionally substituted or interrupted with one or more heteroatoms, this or these chains may be inert to N-substituted imidazolidinone functional groups and nitrile oxides.

[0009] In the sense of the present invention, the term "hydrocarbon chain inert to N-substituted imidazolidinone functional groups and nitrile oxides" is understood to mean a hydrocarbon chain that does not react with either said N-substituted imidazolidinone functional groups or said nitrile oxides. Thus, said hydrocarbon chain inert to said N-substituted imidazolidinone functional groups and said nitrile oxides is preferably an aliphatic hydrocarbon chain that does not have said functional groups or alkenyl or alkynyl functional groups capable of reacting with said groups, i.e. a saturated, linear or branched aliphatic hydrocarbon chain, which is optionally substituted or interrupted by one or more heteroatoms and which contains preferentially 1 to 24 carbon atoms. Preferably, the group A is a C6-C substituted or unsubstituted aliphatic hydrocarbon chain, which is optionally substituted by one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains. 14 arenediyl rings, the hydrocarbon chain of which is optionally substituted or interrupted by one or more heteroatoms. More preferentially, the group A is optionally one or more identical or different, saturated, linear or branched C-C 24 C6-C substituted with aliphatic hydrocarbon chains 14 arenediyl rings, the hydrocarbon chain of which is optionally substituted or interrupted by one or more nitrogen, sulfur or oxygen heteroatoms. Even more preferentially, the group A is optionally C1-C 12 C6-C substituted with one or more identical or different substituents selected from the group consisting of (more preferentially C1-C6, even more preferentially C1-C4) alkyl, OR', -NHR' and -SR' groups; 14 arenediyl ring, R' is C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl groups.

[0010] Preferably, the compound of formula (I) is selected from the compounds of formula (Ia) and (Ib): [ka] During the ceremony, One group selected from R1 to R5 in formula (Ia) and one group selected from R1 to R7 in formula (Ib) represent a group of the following formula (II): [ka] (II) In the formula, E and X are defined as above. The four groups selected from R1 to R5 of formula (Ia) other than the group of formula (II) and the six groups selected from R1 to R7 of formula (Ib) other than the group of formula (II) are identical or different and independently represent a hydrogen atom or, preferably, a saturated, linear or branched aliphatic hydrocarbon chain optionally substituted or interrupted by one or more heteroatoms. Preferably, in the compounds of (Ia) and (Ib), the four groups selected from R1 to R5 of formula (Ia) other than the group of formula (II) and the six groups selected from R1 to R7 of formula (Ib) other than the group of formula (II) are identical or different and independently represent a hydrogen atom or a saturated, linear or branched C1-C aryl group optionally substituted or interrupted by one or more heteroatoms. 24 More preferably, in the compounds (Ia) and (Ib), the four radicals selected from R1 to R5 of formula (Ia) other than the radical of formula (II) and the six radicals selected from R1 to R7 of formula (Ib) other than the radical of formula (II) are identical or different and are each a hydrogen atom, a C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being selected from the group formed by C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl.

[0011] According to a preferred embodiment of the present invention, in formula (Ia), R2 is a group of formula (II) as defined above, and R1, R3, R4 and R5 are identical or different and represent a hydrogen atom or preferably a saturated, linear or branched C1-C1C2 alkyl group, optionally substituted or interrupted by one or more heteroatoms. 24More preferentially, R2 is a group of formula (II) as defined above, and R1, R3, R4 and R5 are identical or different and are a hydrogen atom, a C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 More preferentially in this embodiment, R2 is a group of formula (II) as defined above, R4 is a hydrogen atom, and R1, R3 and R5 are preferably saturated, linear or branched C1-C alkyl, optionally substituted or interrupted by one or more heteroatoms. 24 Even more preferentially, R2 is a group of formula (II) as defined above, R4 is a hydrogen atom, and R1, R3 and R5 are identical or different and are C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl.

[0012] According to another preferred embodiment of the present invention, in formula (Ib), R1 is a group of formula (II) as defined above, and R2 to R7 are identical or different and are each a hydrogen atom or preferably a saturated, linear or branched C1-C aryl group, optionally substituted or interrupted by one or more heteroatoms. 24 More preferentially, R1 is a group of formula (II) as defined above, R2 to R7 are identical or different and are a hydrogen atom, a C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12, more preferentially C1-C6, even more preferentially C1-C4 alkyl. Even more preferentially in this embodiment, R1 is a group of formula (II) as defined above, R2 to R7 are identical and are a hydrogen atom. In the compounds of formulae (I), (Ia) and (Ib), the group E is a divalent hydrocarbon group, which may optionally contain one or more heteroatoms. In the sense of the present invention, the term "divalent hydrocarbon group" is understood to mean a spacer group (or linking group) bridging the group A and the N-substituted imidazolidinone group, which spacer group is saturated or unsaturated, preferably saturated, linear or branched C1-C 24 is a hydrocarbon chain, which may optionally contain one or more heteroatoms, such as, for example, N, O and S. Said hydrocarbon chain may be optionally substituted, provided that the substituents do not react with the nitrile oxide and N-substituted imidazolidinone groups defined above. Preferentially, in the compounds of formulae (I), (Ia) and (Ib), the group E is preferably a saturated, linear or branched C1-C 1 -C 2 -C 3 -C 4 -C 5 -C 6 -C 7 -C 8 -C 9 -C 10 -C 11 -C 12 -C 13 -C 14 -C 15 -C 16 -C 17 -C 18 -C 19 -C 20 -C 21 -C 22 -C 23 -C 24 -C 25 -C 36 -C 26 -C 37 -C 38 -C 39 -C 40 -C 41 -C 52 -C 53 -C 27 -C 38 -C 39 -C 42 -C 54 -C 39 -C 43 -C 55 -C 66 -C 70 -C 71 -C 72 -C 73 -C 84 -C 95 -C 106 -C 117 -C 120 -C 138 -C 14 -C 15 -C 26 -C 16 -C 27 -C 38 -C 28 -C 39 -C 41 -C 29 -C 39 -C 42 -C 54 -C 39 -C 29 -C 39 -C 43 -C 55 -C 39 -C 29 -C 39 -C 41 -C 29 -C 39 -C 42 -C 54 -C 39 -C 29 -C 39 -C 24 , and more preferentially C1-C 10 and even more preferentially a C1-C6 hydrocarbon chain. Preferably, in the compounds of formulae (I), (Ia) and (Ib), the group E is selected from the group consisting of -R-, -NH-R-, -OR- and -SR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 More preferably, in the compounds of formulae (I), (Ia) and (Ib), the group E is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C6 alkylene. 24 , preferably C1-C 10 , and more preferentially C1-C6 alkylene. Even more preferentially, in the compounds of formulae (I), (Ia) and (Ib), the group E is selected from -CH2-, -CH2-CH2-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-, -O-CH2-, -O-CH2-CH2-, -O-CH2-CH2-CH2- and -O-CH2-CH2-CH2-CH2-.

[0013] According to a preferred embodiment, the compound of formula (I) is a compound of formula (Ib). According to this preferred embodiment, in particular, the group E is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 More preferentially, the compound of formula (Ib) as defined above is C1-C6 alkylene and the group X is a chlorine atom. According to this embodiment, more preferentially, the compound of formula (I) is a compound of formula (Ib) as follows: R1 is a group of formula (II), the group E is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene and the group X represents a chlorine atom; and R2 to R7 are the same or different and are each a hydrogen atom or preferably a saturated, linear or branched C1-C alkyl group, optionally substituted or interrupted by one or more heteroatoms. 24 It is an aliphatic hydrocarbon chain. According to this embodiment, even more preferentially, the compound of formula (I) is a compound of formula (Ib) as follows: R1 is a group of formula (II), the group E is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene and the group X represents a chlorine atom; and R2 to R7 are the same or different and are a hydrogen atom, C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl. According to this embodiment, even more preferentially, the compound of formula (I) is a compound of formula (Ib) as follows: R1 is a group of formula (II), the group E is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24, preferably C1-C 10 , more preferentially C1-C6 alkylene and the group X represents a chlorine atom; and R2 to R7 are the same and are hydrogen atoms.

[0014] According to a particular embodiment, the compound of formula (I) is selected from the group consisting of the compounds of formula (III) and formula (IV), more preferentially the compound of formula (III). [ka]

[0015] The rubber compositions according to the invention, comprising at least one compound of formula (I), preferably of formula (Ib) and even more preferentially of formula (III) carrying an N-substituted imidazolidinone group, i.e. a non-associative nitrogen group, optionally previously grafted onto a diene elastomer, surprisingly show a significant reduction in hysteresis, i.e. an improvement in rolling performance. The compounds of formula (I), in particular of formulae (Ia), (Ib), (III) and (IV), can be obtained from a synthesis process comprising the following successive steps: (b1) Reaction of a compound of formula (IX): [ka] (IX) wherein A is as defined above and Y is a nucleophilic group having a compound of formula (X): [ka] (X) In the formula, E is as defined above and Z is a nucleofugic group. In the presence of at least one polar solvent S1, at least one base, at a temperature T1 between 70 and 150° C., a compound of formula (XI) is formed: [ka] (XI) (b2) The compound of formula (XI) is reacted with an aqueous hydroxylamine solution at a temperature T2 of 30 to 70° C. to obtain an oxime compound of formula (XII) below. [ka] (XII) (c) recovering the oxime compound of formula (XII); (d) an oxidation step of the oxime compound of formula (XII) with an oxidizing agent in the presence of at least one organic solvent S2, the content of the oxidizing agent being at least 6 molar equivalents relative to the molar amount of the oxime compound of formula (XII). In the sense of the present application, the term "polar solvent" is understood to mean a solvent with a dielectric constant greater than 2.2. In the sense of the present application, the term "nucleophilic group" is understood to mean a leaving group that removes a bond pair. In the sense of the present application, the term "nucleophilic group" is understood to mean a compound that contains at least one atom with a free pair or one atom with a negative charge.

[0016] As explained above, the method for the synthesis of a compound of formula (I) comprises in particular the successive steps (b1) and (b2). According to a particular embodiment, the two steps (b1) and (b2) are divided into a step for the separation and purification of the compound of formula (XI). According to another embodiment, the two steps (b1) and (b2) are carried out by a one-pot synthesis. That is to say, steps (b1) and (b2) are "one-pot" (two-step one-pot synthesis method), i.e. without separation of the intermediate compound of formula (XI). The method comprises a step (b1) of reaction of a compound of formula (IX) as defined above, bearing a group Y, with a compound of formula (X) as defined above, bearing a group Z. Preferably, the group Y is selected from hydroxyl, thiol, and primary or secondary amine functions. The group Z may be selected from chlorine, bromine, iodine, mesylate, tosylate, acetate, and trifluoromethylsulfonate groups. Said step (b1) of the method is carried out at a temperature T1 between 70 and 150 ° C in the presence of at least one polar solvent S1 and at least one base. According to a particular embodiment of the method, the polar solvent S1 is a water-miscible polar solvent, preferentially a protic solvent. Dimethylformamide (DMF), dimethylsulfoxide (DMSO), 1,3-dimethyl-2-imidazolidinone (DMI), 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone (DMPU), isopropanol, acetonitrile, ethanol, n-butanol and n-propanol are examples of solvents S1 that may be used in the method. Preferably, the protic solvent is an alcoholic solvent.

[0017] Advantageously, the compound of formula (IX) is present in an amount ranging from 5 to 40% by weight, preferably from 10 to 30% by weight, relative to the weight of the solvent. The base may be chosen from alkali metal alkoxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydroxides, alkaline earth metal hydroxides, and mixtures thereof. Advantageously, the following may be added: one or more catalysts selected from silver(I) salt-based catalysts, quaternary ammonium-based phase transfer catalysts, and mixtures thereof; One or more ionic liquids. Preferentially, the base is selected from sodium methoxide, potassium carbonate and sodium hydroxide, more preferentially potassium carbonate. According to a particular embodiment of the process, the molar amount of the base is between 1.5 and 8 molar equivalents, preferably between 2 and 6 molar equivalents relative to the molar amount of the compound of formula (IX). As mentioned above, step (b1) of the process is carried out at a temperature T1 between 70 and 150°C. Preferably, the temperature T1 is between 70 and 120°C, more preferentially between 80 and 110°C. As mentioned above, step (b1) of the process is followed by a step (b2) of adding an aqueous solution of hydroxylamine to the reaction medium containing the compound of formula (XI) at a temperature T2 between 30 and 70°C. Preferentially, the addition of the aqueous solution of hydroxylamine is carried out when the conversion of the compound of formula (IX) is at least 70% by weight. Advantageously, the temperature T2 is between 40 and 60°C.

[0018] The method also includes a step (c) of recovering the oxime compound of formula (XII) as described above. Preferably, the oxime compound of formula (XII) is recovered by precipitation with water, followed by optional washing with water. The method also includes a step (d) of oxidizing the oxime compound of formula (XII) with an oxidizing agent to obtain the compounds of formula (I), particularly preferred compounds, in the presence of at least one organic solvent S2, the amount of oxidizing agent being at least 6 molar equivalents, preferentially 6.5 to 15 molar equivalents, relative to the molar amount of the oxime compound of formula (XII). This amount of oxidizing agent may be added in one or more portions in step (d), preferably in two portions in step (d). Preferably, the oxidizing agent is selected from sodium hypochlorite, N-bromosuccinimide in the presence of a base, and N-chlorosuccinimide in the presence of a base, preferably the oxidizing agent is sodium hypochlorite. Preferentially, the organic solvent S2 is an organic solvent selected from chlorine-based, ester-based, ether-based and alcohol-based solvents, more preferentially selected from dichloromethane, ethyl acetate, butyl acetate, diethyl ether, isopropanol and ethanol, even more preferentially selected from ethyl acetate and butyl acetate. Preferably, the oxime compound of formula (XII) is present in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, relative to the total weight of the combination comprising said oxime compound of formula (XII), said organic solvent S2 and said oxidizing agent. Preferentially, the method comprises, after step (d), a step (e) of recovering the compound of formula (I).

[0019] According to a particular embodiment, the process may comprise, before step (b1), a step (a2) of preparing a compound of formula (X) by reacting a compound of formula (XIII) as follows: [ka] (XIII) During the ceremony, E is as defined above; An agent that allows for the formation of a nucleofugic group Z is used. Preferably, said agent is thionyl chloride. Preferably, step (a2) is carried out in the absence or presence of at least one solvent S4, preferentially a chlorinated solvent, more preferentially dichloromethane. Advantageously, step (a2) is immediately followed by a recovery step (a3) ​​of the compound of formula (X), preferentially by purification with toluene, more preferentially by crystallization of the compound of formula (X) from toluene. Preferentially, the molar content of the compound of formula (I) in the rubber composition according to the invention is in the range of 0.01 to 5 mol %, preferably 0.01 to 1 mol %, more preferentially 0.1 to 1 mol %, irrespective of the distinction between diene or non-diene units. The term "content of the compound of formula (I)" present in the rubber composition, expressed as a molar percentage, is understood to mean the number of compounds of formula (I) present in the rubber composition per 100 units of diene elastomer of the composition. For example, if the content of the compound of formula (I) relative to SBR (styrene / butadiene rubber) is 0.2 mole %, then there will be 0.2 units of the compound of formula (I) per 100 units of SBR styrene and butadiene. If both an elastomer pre-grafted with a compound of formula (I) and a diene elastomer not grafted with a compound of formula (I) are used in the composition, the content of the compound of formula (I) represents the number of grafted compounds of formula (I) per 100 units of diene elastomer, the number of units taking into account both elastomers (grafted and non-grafted), and assuming that no other compounds of formula (I) not pre-grafted are added to the composition.

[0020] Elastomer As mentioned above, the rubber composition of the present invention is based on at least one diene elastomer. A "diene" elastomer (or, without distinction, rubber) should be understood to mean an elastomer, natural or synthetic, which, as is known, is composed at least in part (i.e. homopolymer or copolymer) of diene monomer units (monomers with two conjugated or non-conjugated carbon-carbon double bonds). These diene elastomers can be divided into two categories: "essentially unsaturated" or "essentially saturated". "Essentially unsaturated" is generally understood to mean a diene elastomer which is at least in part derived from a conjugated diene monomer containing more than 15% (mol %) of units of diene origin (conjugated diene). Thus, diene elastomers such as butyl rubber or copolymers of dienes with alpha-olefins of the EPDM type are not included in the above definition and may in particular be described as "essentially saturated" diene elastomers (which have a low or very low content of units of diene origin, always less than 15%).

[0021] Diene elastomers that can be used in the context of the present invention are understood to mean in particular: Any homopolymer of conjugated or non-conjugated diene monomers having 4 to 18 carbon atoms; Any copolymer of a conjugated or non-conjugated diene having from 4 to 18 carbon atoms and at least one other monomer. The other monomers may be ethylene, olefins, or conjugated or non-conjugated dienes. Suitable conjugated dienes are conjugated dienes having 4 to 12 carbon atoms, especially 1,3-dienes, such as in particular 1,3-butadiene and isoprene. Suitable non-conjugated dienes are non-conjugated dienes having 6 to 12 carbon atoms, such as 1,4-hexadiene, ethylidene norbornene, or dicyclopentadiene. Suitable olefins are vinyl aromatic compounds having 8 to 20 carbon atoms, and aliphatic alpha monoolefins having 3 to 12 carbon atoms. Suitable vinyl aromatic compounds are, for example, styrene, ortho-, meta-, or para-methylstyrene, the commercially available "vinyl toluene" mixtures, or para(tert-butyl)styrene. Suitable aliphatic alpha monoolefins are, in particular, acyclic aliphatic alpha monoolefins having 3 to 18 carbon atoms. More specifically, the diene elastomers may be: any homopolymer of a conjugated diene monomer, in particular any homopolymer obtained by polymerization of a conjugated diene monomer having from 4 to 12 carbon atoms; any copolymer obtained by copolymerization of one or more conjugated dienes with one another or with one or more vinyl aromatic compounds having from 8 to 20 carbon atoms; Copolymers of isobutene and isoprene (butyl rubber) and halogenated, especially chlorinated or brominated, forms of such copolymers; Any copolymer obtained by copolymerization of one or more conjugated or non-conjugated dienes with ethylene, with alpha-monoolefins, or with mixtures thereof, such as, for example, elastomers obtained from ethylene, elastomers obtained from propylene and non-conjugated diene monomers of the abovementioned types.

[0022] Preferentially, the diene elastomer is selected from the group consisting of ethylene / propylene / diene monomer (EPDM) copolymers, butyl rubber (IIR), natural rubber (NR), synthetic polyisoprene (IR), polybutadiene (BR), butadiene copolymers, isoprene copolymers, and mixtures of these elastomers.Preferentially, the diene elastomer is selected from the group consisting of ethylene / propylene / diene monomer (EPDM) copolymers, butyl rubber (IIR), natural rubber (NR), synthetic polyisoprene (IR), polybutadiene (BR), butadiene / styrene copolymers (SBR), ethylene / butadiene copolymers (EBR), isoprene / butadiene copolymers (BIR) or isoprene / butadiene / styrene copolymers (SBIR), isobutene / isoprene copolymers (butyl rubber-IIR), isoprene / styrene copolymers (SIR), and mixtures of these elastomers. Preferentially, the diene elastomer is selected from the group consisting of ethylene / propylene / diene monomer copolymers, butyl rubber, and mixtures of these rubbers. Preferentially, the diene elastomer is selected from the group consisting of natural rubber, synthetic polyisoprene, polybutadiene, butadiene copolymers, isoprene copolymers, and mixtures of these elastomers. Even more preferentially, the diene elastomer is selected from the group consisting of natural rubber, synthetic polyisoprene, polybutadiene, butadiene / styrene copolymers, ethylene / butadiene copolymers, isoprene / butadiene copolymers, isoprene / butadiene / styrene copolymers, isobutene / isoprene copolymers, isoprene / styrene copolymers, and mixtures of these elastomers. Preferentially, the diene elastomer is selected from the group consisting of polybutadiene, butadiene copolymers, isoprene copolymers, and mixtures of these elastomers. More preferentially, the diene elastomer is selected from the group consisting of polybutadiene, butadiene / styrene copolymers, ethylene / butadiene copolymers, isoprene / butadiene / styrene copolymers, isobutene / isoprene copolymers, isoprene / styrene copolymers, and mixtures of these elastomers.

[0023] Preferred are polybutadienes, in particular those with a content (mol%) of 1,2 units between 4% and 80% or a content (mol%) of cis-1,4 units greater than 80%, polyisoprene, butadiene / styrene copolymers, in particular those with a Tg (glass transition temperature (Tg measured according to ASTM D3418 (2015)) between 0° C. and −90° C., and more particularly between −10° C. and −70° C., a styrene content between 1% and 60% by weight, and more particularly between 20% and 50%, a content (mol%) of 1,2 bonds in the butadiene part between 4% and 75% and a content (mol%) of trans-1,4 bonds between 10 and 80%, butadiene / isoprene copolymers, in particular those with an isoprene content between 5% and 90% by weight. % by weight and a Tg between -40°C and -80°C, or isoprene / styrene copolymers, particularly those having a styrene content between 5% and 50% by weight and a Tg between -5°C and -50°C. In the case of butadiene / styrene / isoprene copolymers, the styrene content is between 5% and 50% by weight, and more particularly between 10% and 40%, the isoprene content is between 15% and 60% by weight, and more particularly between 20% and 50%, the butadiene Particularly suitable are any butadiene / styrene / isoprene copolymers having an ene content between 5% and 50% by weight, and more particularly between 20% and 40%, a content (mol%) of 1,2 units in the butadiene part between 4% and 85%, a content (mol%) of trans-1,4 units in the butadiene part between 6% and 80%, a content (mol%) of 1,2- and 3,4 units in the isoprene part between 5% and 70%, and a content (mol%) of trans-1,4 units in the isoprene part between 10% and 50%, and more generally a Tg between -5°C and -70°C. The diene elastomers may have any microstructure, depending on the polymerization conditions used. These polymers may be, for example, block, random, sequential or microsequential polymers and may be prepared in dispersion, emulsion or solution. They may be bonded and / or star-branched, for example by silicon or tin atoms linking the polymer chains.

[0024] In a first preferred embodiment of the invention, the rubber composition of the invention is based on at least one diene elastomer and at least one compound of formula (I) as defined above, which has been previously grafted onto the diene elastomer. The term "diene elastomer previously grafted with at least one compound of formula (I)" is understood to mean a diene elastomer having a functional group introduced into its chain, in particular an N-substituted imidazolidinone functional group. In practice, the modified diene elastomer is obtained by grafting reaction of at least one compound of formula (I) which has a substituted N-imidazolidinone functional group and which has a functional group capable of forming a covalent bond with the unsaturated portion of the chain of the initial diene elastomer, this functional group being a nitrile oxide. During the grafting reaction, the nitrile oxide functional group or groups of the grafted compound form a covalent bond with the unsaturated portion or portions of the chain of the diene elastomer. The term "unsaturated portion" is understood to mean a multiple covalent bond between two carbon atoms. This multiple covalent bond may be a carbon-carbon double bond or a carbon-carbon triple bond, preferably a carbon-carbon double bond. In the sense of the present invention, the term "initial diene elastomer chain" is understood to mean a diene elastomer chain before the grafting reaction, which chain has at least one unsaturated moiety, more preferentially at least two unsaturated moieties, capable of reacting with a compound having a nitrile oxide functional group. The initial diene elastomer is therefore the diene elastomer which serves as the starting reactant during the grafting reaction. The grafting reaction makes it possible, starting from the initial elastomer, to obtain modified diene elastomers, also called pregrafted diene elastomers. The method for pregrafting a diene elastomer with a compound of formula (I), preferably with a compound of formula (Ib) and more preferentially with a compound of formula (III), is described hereinafter.

[0025] According to a second preferred embodiment of the invention, the rubber composition of the invention is based on at least one diene elastomer and at least one compound of formula (I) as defined above. The rubber composition of the invention can therefore contain a single diene elastomer grafted with a compound of formula (I) (grafted before being introduced into the composition or grafted by reacting with a compound of formula (I) during the preparation of the composition) or a mixture of several diene elastomers (all grafted, or some grafted and others not). The one or more other diene elastomers, optionally previously grafted with at least one compound of formula (I), used as a blend with the diene elastomer of the composition of the invention, are conventional diene elastomers as described above, whether star-branched, bonded or functionalized. The diene elastomer of the composition of the invention, optionally previously grafted with at least one compound of formula (I), may be used in combination with any type of synthetic elastomer other than diene elastomers, and even in combination with polymers other than elastomers.

[0026] Reinforcing Fillers As mentioned above, the rubber composition of the present invention is based on at least one reinforcing filler. The reinforcing filler may be any type of "reinforcing" filler known to be capable of reinforcing rubber compositions that can be used, in particular by tire manufacturers, such as organic fillers, such as carbon black, inorganic fillers, such as silica, or a mixture of these two types of fillers. Advantageously, the reinforcing filler is selected from carbon black, reinforcing inorganic fillers, and mixtures of carbon black and inorganic fillers. All carbon blacks are suitable as carbon blacks, in particular the blacks that are usually used in tires or their treads. Among the blacks, more particular mention may be made of reinforcing carbon blacks of the 100, 200 and 300 series, or blacks of the 500, 600 or 700 series (ASTM D-1765-2017 grades), such as N115, N134, N234, N326, N330, N339, N347, N375, N550, N683 and N772 blacks. These carbon blacks may be used in the separated form available commercially or in any other form, for example as carriers for some of the rubber additives used. The carbon blacks may be premixed, for example in the form of masterbatches, in diene elastomers, in particular isoprene elastomers (see, for example, WO 97 / 36724 or WO 99 / 16600). As examples of organic fillers other than carbon black, mention may be made of the functionalized polyvinyl organic fillers described, for example, in WO 2006 / 069792, WO 2006 / 069793, WO 2008 / 003434 and WO 2008 / 003435. In the present specification, "reinforcing inorganic filler" should be understood to mean any inorganic or mineral filler, regardless of its color or origin (natural or synthetic), also known as a "white" filler, "transparent" filler or "non-black" filler in contrast to carbon black, which is capable by itself of reinforcing rubber compositions for the manufacture of tires, without the aid of any intermediate coupling agent. As is known, some reinforcing inorganic fillers may be characterized in particular by the presence of hydroxyl (-OH) groups on their surface.Siliceous mineral fillers, preferentially silica (SiO2), or aluminous mineral fillers, especially alumina (Al2O3), are particularly suitable as reinforcing inorganic fillers.

[0027] Preferably, the reinforcing inorganic filler is silica. The silica used may be any reinforcing silica known to those skilled in the art, in particular one having a BET specific surface area and a CTAB specific surface area of ​​450 m 2 / g, preferably 30 to 400m 2 / g, especially 60-300m 2 The silica may be any precipitated or fumed silica within the range of 0.1 to 0.5 μg / g. Any type of precipitated silica may be used, in particular highly disperse precipitated silica (referred to as "HDS" instead of "highly disperse" or "highly disperse silica"). These precipitated silicas, whether highly disperse or not, are well known to those skilled in the art. For example, mention may be made of the silicas described in WO 03 / 016215 and WO 03 / 016387. Among the commercially available HDS silicas in particular, the Ultrasil® 5000GR and Ultrasil® 7000GR silicas from Evonik, or the Zeosil® 1085GR, Zeosil® 1115MP, Zeosil® 1165MP, Zeosil® Premium 200MP and Zeosil® HRS1200MP silicas from Solvay may be used. As non-HDS silicas, the following commercially available silicas may be used: Ultrasil® VN2GR and Ultrasil® VN3GR silicas from Evonik, Zeosil® 175GR silica from Solvay, or Hi-Sil EZ120G(-D), Hi-Sil EZ160G(-D), Hi-Sil EZ200G(-D), Hi-Sil243LD, Hi-Sil210, and Hi-Sil HDP320G silicas from PPG. The physical state in which the reinforcing inorganic filler is provided is not important and may be in the form of powder, beads such as microbeads, granules, or any other suitable densified form. Of course, reinforcing inorganic fillers are also understood to mean mixtures of various reinforcing inorganic fillers, in particular mixtures of the silicas mentioned above.

[0028] As an alternative to the above-mentioned reinforcing inorganic fillers, reinforcing fillers of another nature may be used, which may be covered with an inorganic layer such as silica or contain functional groups, especially hydroxyl groups, on the surface of the filler, and which will require the use of a coupling agent to establish a bond between the reinforcing filler and the diene elastomer, as will be understood by those skilled in the art. As an example of carbon black partially or completely covered with silica, mention may be made of silica-modified carbon blacks, such as, but not limited to, Ecoblack® type fillers of the CRX2000 or CRX4000 series of Cabot Corporation. Those skilled in the art will know how to adjust the reinforcing filler content depending on the application, in particular depending on the type of tire involved, such as motorcycle, car or utility vehicle tires, such as vans and large cars. Preferably, this total content of reinforcing fillers (carbon black and / or reinforcing inorganic fillers, preferably carbon black and / or silica) is in the range of 10 to 200 phr, more preferentially 30 to 180 phr, and even more preferentially 40 to 160 phr, the optimum total content depending on the intended specific application, as is known. According to an alternative form of the invention, the reinforcing fillers are predominantly other than carbon black, i.e. more than 50% by weight of the total mass of the reinforcing fillers are one or more reinforcing fillers other than carbon black, in particular reinforcing inorganic fillers such as silica, and may in fact consist exclusively of such fillers (i.e. consist exclusively of reinforcing inorganic fillers, preferably consist exclusively of silica). If carbon black is also present in this alternative form, it may be used in a content of less than 20 phr, more preferentially less than 10 phr (for example between 0.5 phr and 20 phr, in particular 1 to 10 phr).

[0029] If the reinforcing filler comprises a reinforcing inorganic filler that requires the use of a coupling agent to establish a bond between the reinforcing filler and the diene elastomer, the rubber composition of the present invention usually additionally comprises an agent capable of effectively forming this bond. If silica is present as a reinforcing filler in the rubber composition of the present invention, an organosilane may be used as a coupling agent. Preferentially, the organosilane is selected from the group consisting of organosilane polysulfides (symmetrical or asymmetrical), such as bis(3-triethoxysilylpropyl)tetrasulfide (abbreviated TESPT, sold under the name Si69 by Evonik) or bis(3-triethoxysilylpropyl)disulfide (abbreviated TESPD, sold under the name Si75 by Evonik), polyorganosiloxanes, mercaptosilanes, blocked mercaptosilanes, such as S-(3-(triethoxysilyl)propyl)octanethioate (sold under the name NXT Silane by Momentive). More preferentially, the organosilane is an organosilane polysulfide. In the composition of the present invention, the content of the coupling agent is advantageously less than 20 phr, and it is generally understood that it is desirable to use as little as possible. The content of the coupling agent is preferentially between 0.5 phr and 12 phr. The presence of the coupling agent depends on the presence of the reinforcing inorganic filler. It is usually about 0.5 to 15% by weight relative to the amount of the reinforcing inorganic filler.

[0030] chemical crosslinking system The rubber composition of the invention is also based on at least one chemical crosslinking system. The crosslinking system may be of any type known to the person skilled in the art in the field of rubber compositions for tires. It may in particular be based on sulfur and / or peroxides and / or bismaleimides. Preferentially the crosslinking system is based on sulfur, in which case it is called a vulcanization system. The sulfur may be provided in any form, in particular in the form of molecular sulfur or sulfur donors. At least one vulcanization accelerator is also preferentially present, and optionally, also preferentially, various known vulcanization activators may be used, such as zinc oxide, stearic acid or equivalent compounds, such as stearates and salts of transition metals, guanidine derivatives (in particular diphenylguanidine), or also known vulcanization retarders. Sulfur is used in a preferential content of between 0.5 and 12 phr, in particular between 0.5 and 5 phr. Vulcanization accelerators are used in a preferential content of between 0.5 phr and 10 phr, more preferentially between 0.5 and 5.0 phr.

[0031] As accelerators, any compound capable of functioning as a vulcanization accelerator for diene elastomers in the presence of sulfur may be used, in particular thiazole accelerators and their derivatives, or sulfenamides, thiurams, dithiocarbamates, dithiophosphates, thioureas, and xanthates.As examples of such accelerators, the following compounds may be mentioned in particular: 2-mercaptobenzothiazyl disulfide (abbreviated as "MBTS"), N-cyclohexyl-2-benzothiazole sulfenamide ("CBS"), N,N-dicyclohexyl-2-benzothiazole sulfenamide ("DCBS"), N-(tert-butyl)-2-benzothiazole sulfenamide ("TBBS"), N-(tert-butyl)-2-benzothiazole sulfenimide ("TBSI"), tetrabenzyl thiuram disulfide ("TBZTD"), zinc dibenzyl dithiocarbamate ("ZBEC"), and compounds of these compounds. Peroxide compounds that may be used as chemical crosslinking systems may include acyl peroxides such as benzoyl peroxide or p-chlorobenzoyl peroxide, ketone peroxides such as methyl ethyl ketone peroxide, peroxyesters such as t-butyl peracetate, t-butyl peroxybenzoate, and t-butyl peroxyphthalate, alkyl peroxides such as dicumyl peroxide, di(t-butyl)peroxybenzoate, and 1,3-bis(t-butylperoxyisopropyl)benzene, or hydroperoxides such as t-butyl hydroperoxide.

[0032] Plasticizer According to an embodiment, the rubber composition may additionally comprise at least one plasticizer. As known to those skilled in the art of rubber compositions for tires, this plasticizer is preferably selected from high glass transition temperature (Tg) hydrocarbon resins, low Tg hydrocarbon resins, plasticizing oils, and mixtures thereof. Preferably, the plasticizer is selected from high Tg hydrocarbon resins, plasticizing oils, and mixtures thereof. By definition, high Tg hydrocarbon resins are solid at ambient temperature and pressure (20° C., 1 atm), whereas plasticizing oils are liquid at ambient temperature and low Tg hydrocarbon resins are viscous at ambient temperature. The total content of plasticizers in the composition is in the range of 1 to 150 phr, preferably in the range of 2 to 120 phr. Hydrocarbon resins, also known as plasticizing hydrocarbon resins, are essentially polymers based on carbon and hydrogen, well known to those skilled in the art, but may contain other types of atoms, such as oxygen, which may be used in polymer matrices, especially as plasticizers or tackifiers. They are essentially at least partially miscible (i.e. compatible) in the content in which they are used with the polymer composition for which they are intended, so as to function as true diluents. They are described, for example, in the work "Hydrocarbon Resins" by R. Mildenberg, M. Zander and G. Collin (New York, VCH, 1997, ISBN 3-527-28617-9), where their application in the field of tire rubber is addressed in chapter 5 (5.5. "Rubber Tires and Mechanical Goods"). As is known, these hydrocarbon resins may be described as thermoplastic resins, in the sense that they soften and can be molded when heated. The softening point of the hydrocarbon resins is measured according to standard ISO 4625 (ring and ball method). The Tg is measured according to standard ASTM D3418 (2015).The macrostructure (Mw, Mn, and PI) of the hydrocarbon resins is determined by size exclusion chromatography (SEC) (solvent: tetrahydrofuran; temperature: 35°C; concentration: 1 g / L; flow rate: 1 mL / min; solution filtered through a filter with porosity of 0.45 μm before injection; Moore calibration with polystyrene standards; set of three Waters columns in series (Styragel HR4E, HR1, and HR0.5); detection by a differential refractometer (Waters2410) and the associated operating software (Waters Empower).

[0033] Hydrocarbon resins may be aliphatic or aromatic, or aliphatic / aromatic, i.e. based on aliphatic and / or aromatic monomers. They may be natural or synthetic, and may or may not be petroleum based (if they are petroleum based, they are also known as petroleum resins). Suitable examples of aromatic monomers include styrene, alpha-methylstyrene, indene, ortho-, meta- or para-methylstyrene, vinyltoluene, para-(tert-butyl)styrene, methoxystyrene, chlorostyrene, vinylmesitylene, divinylbenzene, vinylnaphthalene, or the C9 cut (or, more generally, C8-C 10 Preferably, the vinyl aromatic monomer is styrene, or any vinyl aromatic monomer derived from a C9 cut (or, more generally, a C8-C 10 According to a particularly preferred embodiment, the plasticizing hydrocarbon resin is selected from the group consisting of cyclopentadiene (abbreviated CPD) or dicyclopentadiene (abbreviated DCPD) homopolymer or copolymer resins, terpene homopolymer or copolymer resins, terpene / phenol homopolymer or copolymer resins, C5 cut homopolymer or copolymer resins, C9 cut homopolymer or copolymer resins, α-methylstyrene homopolymer or copolymer resins, and mixtures of these resins.

[0034] As is known, a high Tg hydrocarbon resin is a thermoplastic hydrocarbon resin, having a Tg above 20° C. Preferably, a high Tg plasticized hydrocarbon resin exhibits at least one of the following characteristics: Tg is higher than 30°C; a number average molecular weight (Mn) between 300 g / mol and 2000 g / mol, more preferentially between 400 g / mol and 1500 g / mol; A polydispersity index (PI) less than 3, more preferentially less than 2 (for the record, PI=Mw / Mn, where Mw is the weight average molecular weight). More preferentially, this high Tg plasticized hydrocarbon resin exhibits all the preferential characteristics described above. The preferential high Tg hydrocarbon resins described above are well known to those skilled in the art and are commercially available, for example: Polylimonene resin: available from DRT under the name Dercolyte L120 (Mn=625 g / mol; Mw=1010 g / mol; PI=1.6; Tg=72° C.) or from Arizona Chemical Company under the name Sylvagum TR7125C (Mn=630 g / mol; Mw=950 g / mol; PI=1.5; Tg=70° C.); C5 cut / vinyl aromatic copolymer resins, especially C5 cut / styrene or C5 cut / C9 cut copolymer resins: available from Neville Chemical Company under the names Super Nevtac 78, Super Nevtac 85, and Super Nevtac 99, from Goodyear Chemicals under the name Wingtack Extra, from Kolon under the names Hikorez T1095 and Hikorez T1100, or from Exxon under the names Escorez 2101 and Escorez 1273; Limonene / styrene copolymer resins: available from DRT under the name Dercolyte TS105, and from Arizona Chemical Company under the name ZT115LT and ZT5100.

[0035] The plasticizer may include extender oils (or plasticizing oils) that are liquid at 20° C. and are called “low Tg” plasticizers, i.e., their Tg is, by definition, lower than −20° C., preferably lower than −40° C. Any extender oil, aromatic or non-aromatic, with known plasticizing properties for elastomers may be used. These oils, which are somewhat viscous, are liquid at ambient temperature (i.e., materials that can ultimately assume the shape of the container, just to be sure), unlike high Tg hydrocarbon resins, which are solid in nature, especially at ambient temperature (20° C.). Particularly suitable are plasticizing oils selected from the group consisting of naphthenic oils (low or high viscosity, in particular hydrogenated or non-hydrogenated), paraffinic oils, MES (medium extraction solvates) oils, TDAE (treated distillate aromatic extract) oils, RAE (residual aromatic extract) oils, TRAE (treated residual aromatic extract) oils, SRAE (safe residual aromatic extract) oils, mineral oils, vegetable oils, ether plasticizers, ester plasticizers, sulfonate ester plasticizers, and mixtures of these compounds.

[0036] Additives The rubber composition according to the invention may also comprise all or part of the usual additives and processing aids known to those skilled in the art and generally used in rubber compositions for tires, in particular for treads, such as, for example, non-reinforcing fillers, pigments, protective agents such as anti-ozone waxes, chemical antiozonants or antioxidants, anti-fatigue agents, or reinforcing resins (as described, for example, in WO 02 / 10269).

[0037] Method for producing rubber composition according to the present invention The rubber composition according to the invention is produced in a suitable mixer using two successive preparation stages well known to the person skilled in the art: the first stage is a thermomechanical operation or kneading at high temperatures ("non-productive" stage) with a maximum temperature ranging from 130 to 200°C, preferably from 145 to 185°C, followed by a second stage (also called "productive" stage) at lower temperatures, usually below 120°C, for example between 30°C and 100°C, in which finishing stage the chemical crosslinking system is mixed in. In general, all the basic constituents of the composition of the invention, except the chemical crosslinking system, i.e. the compound of formula (I) in the selected embodiment, preferably the compound of formula (Ib), more preferentially the compound of formula (III), the reinforcing filler(s) and, if necessary, the coupling agent, are intimately mixed by kneading into the diene elastomer(s), if appropriate, in the first "non-productive" stage. That is, at least these various basic components are charged into a suitable mixer, for example a standard internal mixer (for example of the "Banbury" type), and are thermomechanically kneaded in one or more steps until a maximum temperature is reached in the range of 130-200° C., preferably in the range of 145-185° C. The total kneading time in this non-productive phase is generally between 2 and 10 minutes.

[0038] The second stage ("productive" stage), which is generally a mechanical operation, is carried out in an external mixer such as an open mill, after cooling the mixture obtained in the first non-productive stage, usually to a temperature below 120°C, for example between 30°C and 100°C. The crosslinking system is then mixed in, after which the combination is mixed for a few minutes, for example between 5 and 15 minutes. The final composition thus obtained is then calendered, for example in the form of plates or plaques, in particular for laboratory characterization, or extruded in the form of semi-finished rubber products (or molded elements) that can be used, for example, as tire treads. The composition can be either in the pre-cured state (before crosslinking or vulcanization) or in the cured state (after crosslinking or vulcanization), and can be a semi-finished product that can be used in tires. The crosslinking of the composition can be carried out in a manner known to the person skilled in the art, for example at temperatures and pressures between 130°C and 200°C.

[0039] According to a first embodiment of the invention, before the preparation of the rubber composition, the diene elastomer is grafted with a compound of formula (I), preferably with a compound of formula (Ib) and more preferentially with a compound of formula (III). In this case, it is therefore the grafted diene elastomer that is introduced in the first "non-productive" stage. According to this first embodiment of the process, the process therefore comprises the following steps: modifying the diene elastomer by solution or bulk grafting with a compound of formula (I) as defined above, preferably with a compound of formula (Ib) and more preferentially with a compound of formula (III); mixing the diene elastomer thus grafted with a compound of formula (I) (or with a preferred compound) with all the basic constituents of the composition, except the reinforcing filler and the chemical crosslinking system, and kneading the combined mixture thermomechanically one or more times until a maximum temperature is reached in the range of 130-200°C, preferably 145-185°C; cooling the mixture obtained in the previous step to a temperature below 100°C; followed by incorporating a chemical crosslinking system; Mixing the mixture from the previous step until the maximum temperature is not more than 120°C; then, optionally, The rubber composition thus obtained is then extruded or calendered. Advantageously, the steps of this first embodiment of the method are consecutive.

[0040] The grafting of the diene elastomer is carried out by reaction of said diene elastomer with a nitrile oxide of a compound of formula (I), preferably of formula (Ib), more preferentially of formula (III). During this reaction, the nitrile oxide group forms a covalent bond with the polymer chain. The grafting of the compound of formula (I), preferably of formula (Ib), more preferentially of formula (III), is carried out by [3+2] cycloaddition of the nitrile oxide and desaturation of the initial polymer chain. The mechanism of [3+2] cycloaddition is explained in WO 2012 / 007441. The grafting of the compound of formula (I), preferably of formula (Ib), more preferentially of formula (III), onto the diene elastomer may be carried out in bulk, for example in an external mixer such as an extruder, an internal mixer or an open mill. It may also be carried out continuously or batchwise in solution. The diene elastomer thus modified may be separated from the solution by any type of means known to those skilled in the art, in particular by steam stripping. According to the invention, the diene elastomer has along its chain one or more pendant groups resulting from the reaction of grafting of a compound of formula (I) as defined above, preferably of formula (Ib) and more preferentially of formula (III). Advantageously, these pendant groups are randomly distributed along the chain.

[0041] According to a preferred embodiment, the molar degree of grafting of the compounds of formula (I), preferably of formula (Ib) and more preferentially of formula (III) is in the range of 0.01-5%, preferably of 0.01-1% and more preferentially of 0.1-1%. The term "molar degree of grafting" is understood to mean the number of moles of the compounds of formula (I), preferably of formula (Ib) and more preferentially of formula (III) grafted onto the diene elastomer per 100 moles of monomer units constituting the diene elastomer. The molar degree of grafting can be determined by conventional analytical methods for diene elastomers, e.g. 1 It may be determined by 1 H NMR analysis.

[0042] According to a second embodiment of the invention, the grafting of the diene elastomer with the compound of formula (I), preferably with the compound of formula (Ib) and even more preferentially with the compound of formula (III), is carried out simultaneously with the preparation of the rubber composition. In this case, both the diene elastomer not yet grafted and the compound of formula (I) (or the preferred compound) are introduced in a first "non-productive" stage. Preferentially, in this same non-productive stage, the reinforcing filler is subsequently added, so as not to cause side reactions with the compound of formula (I). Thus, according to a second embodiment of the process, the process comprises the following steps: During bulk compounding, the compound of formula (I) as defined above, preferably the compound of formula (Ib) and more preferentially the compound of formula (III), is mixed into the diene elastomer at a temperature in particular ranging from 60 to 140°C and for a time in particular ranging from 30 seconds to 3 minutes; these temperature and time conditions advantageously achieve a grafting rate of at least 60%, more preferentially at least 80%, preferably followed by the mixing of the reinforcing filler, as well as all the basic constituents of the composition except the chemical crosslinking system, and the combined mixture is thermomechanically kneaded one or more times until a maximum temperature is reached in the range of 130 to 200°C, preferably 145 to 185°C; cooling the combination to a temperature below 100°C; followed by incorporating a chemical crosslinking system; kneading the combined mixture until the maximum temperature is not more than 120°C; and optionally The rubber composition thus obtained is then extruded or calendered. Advantageously, the steps of this second embodiment of the method are consecutive.

[0043] The rubber composition according to the invention additionally comprises a compound of formula (V) According to an alternative form of the invention, the rubber composition additionally comprises at least one compound of formula (V) optionally pre-grafted to a diene elastomer, the chains of which may already have been grafted with at least one compound of formula (I) as defined above: [ka] (V) During the ceremony, A1 is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; and ·E1 is a divalent hydrocarbon group optionally containing one or more heteroatoms.

[0044] Preferably, the group A1 of the compound of formula (V) is a C6-C substituted, optionally with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains. 14 arenediyl rings, the hydrocarbon chain of which is optionally substituted or interrupted by one or more heteroatoms. More preferentially, the group A1 is optionally one or more identical or different saturated, linear or branched C1-C 24 C6-C substituted with hydrocarbon chain 14 arenediyl rings, the hydrocarbon chain of which is optionally substituted or interrupted by one or more nitrogen, sulfur or oxygen heteroatoms. Even more preferentially, the group A1 is optionally C1-C 12 C6-C substituted with one or more identical or different substituents selected from the group consisting of (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups; 14 arenediyl ring, R' is C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl groups.

[0045] Preferably, the compound of formula (V) is selected from the compounds of formula (Va) and (Vb): [ka] During the ceremony, R8 to R in formula (Va) 12 and R8 to R in formula (Vb): 14 One group selected from represents a group of formula (VI): [ka] (VI) wherein E1 is as defined above; and R8 to R in formula (Va) 12 four groups other than the group of formula (VI), and R to R of formula (Vb) 14 The six groups other than the one representing the group of formula (VI), selected from the group consisting of: Preferably, in the compounds of (Va) and (Vb), the four groups selected from R1 to R5 of formula (Va) other than the group of formula (VI) and the six groups selected from R1 to R7 of formula (Vb) other than the group of formula (VI) are identical or different and independently represent a hydrogen atom or a saturated, linear or branched C1-C aryl group optionally substituted or interrupted by one or more heteroatoms. 24 More preferably, in the compounds (Va) and (Vb), the four radicals selected from R1 to R5 of formula (Va) other than the radical of formula (VI) and the six radicals selected from R1 to R7 of formula (Vb) other than the radical of formula (VI) are identical or different and are each a hydrogen atom, a C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being selected from the group formed by C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl.

[0046] According to a preferred embodiment of the present invention, in formula (Va), R9 is a group of formula (VI) as defined above, R8, R 10 , R 11 , and R 12 are identical or different and are hydrogen atoms or, preferably, saturated, linear or branched C-C alkyl groups, optionally substituted or interrupted by one or more heteroatoms. 24More preferentially, R9 is a group of formula (VI) as defined above, R8, R 10 , R 11 , and R 12 are the same or different and are a hydrogen atom, C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 More preferentially in this embodiment, in formula (Va), R9 is a group of formula (VI) as defined above, R 11 is a hydrogen atom, R, R 10 , and R 12 is preferably a saturated, linear or branched C-C alkyl group, optionally substituted or interrupted by one or more heteroatoms. 24 Even more preferentially, R9 is a group of formula (VI) as defined above, R 11 is a hydrogen atom, R, R 10 , and R 12 are the same or different, C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl.

[0047] According to another preferred embodiment of the invention, in formula (Vb), R8 is a group of formula (VI) as defined above, and R9 to R 14 are identical or different and are hydrogen atoms or, preferably, saturated, linear or branched C-C alkyl groups, optionally substituted or interrupted by one or more heteroatoms. 24 More preferentially, R8 is a group of formula (VI) as defined above and R9 to R 14 are the same or different and are a hydrogen atom, C1-C 12(more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 More preferentially in this embodiment, R8 is a group of formula (VI) as defined above, R9 to R 14 are identical and are hydrogen atoms. In the compounds of formulae (V), (Va) and (Vb), the group E1 is a divalent hydrocarbon group, which may optionally contain one or more heteroatoms. In the sense of the present invention, the term "divalent hydrocarbon group" is understood to mean a spacer group (or linking group) bridging the group A1 and the imidazolidinone group, this spacer group being saturated or unsaturated, preferably saturated, linear or branched C1-C 24 is a hydrocarbon chain, which may optionally contain one or more heteroatoms, such as, for example, N, O and S. Said hydrocarbon chain may be optionally substituted, provided that the substituents do not react with the nitrile oxide and imidazolidinone groups defined above. Preferentially, in the compounds of formulae (V), (Va) and (Vb), the group E1 is preferably a saturated, linear or branched C1-C cyclic ring, optionally interrupted by one or more nitrogen, sulfur or oxygen atoms. 24 , and more preferentially C1-C 10 , and even more preferentially a C1-C6 hydrocarbon chain. Preferably, in the compounds of formulae (V), (Va) and (Vb), the group E1 is selected from the group consisting of -R-, -NH-R-, -OR- and -SR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 More preferably, in the compounds of formulae (V), (Va) and (Vb), the group E1 is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C6 alkylene. 24 , preferably C1-C 10, and more preferentially C1-C6 alkylene. Even more preferentially, in the compounds of formulae (V), (Va) and (Vb), the group E1 is selected from -CH2-, -CH2-CH2-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-, -O-CH2-, -O-CH2-CH2-, -O-CH2-CH2-CH2- and -O-CH2-CH2-CH2-CH2-.

[0048] According to a preferred embodiment, the compound of formula (V) is a compound of formula (Vb): In this preferred embodiment, in particular, the group E1 is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 Preference is given to compounds of formula (Vb) as defined above, which is more preferentially C1-C6 alkylene. According to this embodiment, more preferentially still, the compound of formula (V) is a compound of formula (Vb) as follows: R8 is a group of formula (VI), the group E1 is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene; and R9~R 14 are identical or different and are hydrogen atoms or, preferably, saturated, linear or branched C-C alkyl groups, optionally substituted or interrupted by one or more heteroatoms. 24 It is an aliphatic hydrocarbon chain. According to this embodiment, even more preferentially, the compound of formula (V) is a compound of formula (Vb) as follows: R8 is a group of formula (VI), the group E1 is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene; and R9~R 14 are the same or different and are a hydrogen atom, C1-C 12(more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, and even more preferentially C1-C4 alkyl. According to this embodiment, even more preferentially, the compound of formula (V) is a compound of formula (Vb) as follows: R8 is a group of formula (VI), the group E1 is selected from the group consisting of -R- and -OR-, R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene; and R9~R 14 are identical and are hydrogen atoms.

[0049] According to a preferred embodiment, the compound of formula (V) is selected from the group consisting of the compounds of formula (VII) and of formula (VIII), and even more preferentially is the compound of formula (VII): [ka] The compounds of formula (V), in particular the compounds of formula (Vb) and (VII), may be synthesized, for example, as described in WO 2019007881. Preferentially, the molar content of the compound of formula (V), preferably the compound of formula (Vb), more preferentially the compound (VII), in the rubber composition of the present invention, is in the range of 0.01 to 5 mol%, preferably 0.01 to 1 mol%, more preferentially 0.1 to 1 mol%, regardless of whether it is a diene unit or a non-diene unit.

[0050] According to a preferred embodiment, the rubber composition of the invention comprises at least one compound of formula (Ib) as defined above, and at least one compound of formula (Vb) as defined above, said compounds being optionally previously grafted to a diene elastomer. Preferably, in this embodiment, the rubber composition of the invention comprises at least: The compound of formula (Ib) having R1 is a group of formula (II), in which the group E is selected from the group consisting of -R- and -OR-, and R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferentially C1-C6 alkylene, and the group X being a chlorine atom, and R2 to R7, which may be the same or different, are each preferably a hydrogen atom, a C1-C6 alkylene. 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, even more preferentially C1-C4 alkyl; and The compound of formula (Vb) having R8 is a group of formula (VI), in which the group E1 is selected from the group consisting of -R- and -OR-, and R is a linear or branched C1-C 24 , preferably C1-C 10 , more preferably C1-C6 alkylene, and R9 to R 14 are hydrogen atoms, C1-C 12 (more preferentially C1-C6, even more preferentially C1-C4) alkyl, -OR', -NHR' and -SR' groups, R' being C1-C 12 , more preferentially C1-C6, even more preferentially C1-C4 alkyl; and Said compound is optionally pre-grafted to a diene elastomer. Even more preferentially, in this embodiment, the rubber composition of the present invention comprises at least one compound of formula (III) and at least one compound of formula (VII), optionally pre-grafted to a diene elastomer.Surprisingly, when the rubber composition of the present invention comprises at least one compound of formula (I) and at least one compound of formula (V), preferably at least one compound of formula (Ib) and at least one compound of formula (Vb), and even more preferentially a compound of formula (III) and at least one compound of formula (VII), optionally pre-grafted to a diene elastomer, it shows the advantage of an improved stiffness / hysteresis trade-off before curing compared to prior art rubber compositions.

[0051] Preparation of the rubber composition of the present invention additionally containing a compound of formula (V) According to a first embodiment of these compositions, before the preparation of the rubber composition, the diene elastomer is grafted with compounds of formula (I) and (V), preferably with compounds of formula (Ib) and (Vb), more preferentially with compounds of formula (III) and (VII). In this case, it is therefore the diene elastomer grafted with compounds of formula (I) and (V) that is introduced in the first "non-productive" stage. According to this first embodiment of the process, it therefore comprises the following steps: modifying the diene elastomer by solution or bulk grafting of the compounds of formula (I) and (V) as defined above, preferably the compounds of formula (Ib) and formula (Vb), more preferentially the compounds of formula (III) and the compounds of formula (VII); mixing the diene elastomer thus grafted with the compounds of formula (I) and formula (V) (or preferred compounds) with all the basic constituents of the composition, except the reinforcing filler and the chemical crosslinking system, and kneading the combined mixture thermomechanically one or more times until a maximum temperature is reached in the range of 130-200°C, preferably 145-185°C; cooling the mixture obtained in the previous step to a temperature below 100°C; followed by incorporating a chemical crosslinking system; Mixing the mixture from the previous step until the maximum temperature is not more than 120°C; then, optionally, The rubber composition thus obtained is then extruded or calendered. Advantageously, the steps of this first embodiment of the method are consecutive.

[0052] The grafting of the diene elastomer is carried out by reaction of said diene elastomer with the nitrile oxide of the compound of formula (I) and with the nitrile oxide of the compound of formula (V). As mentioned above, the grafting of the compounds of formula (I) and (V) (or the preferred compounds mentioned above) is carried out by [3+2] cycloaddition of the nitrile oxide and by unsaturation of the chains of the initial diene elastomer. The grafting of the compounds of formula (I) and (V), preferably of formula (Ib) and (Vb), and more preferentially of formula (III) and (VII), onto the initial polymer may be carried out in bulk, for example in an external mixer such as an extruder, an internal mixer or an open mill. It may also be carried out continuously or batchwise in solution. The diene elastomer thus modified may be separated from the solution by any type of means known to the skilled person, in particular by steam stripping. The compounds of formulae (I) and (V), preferably those of formulae (Ib) and (Vb), and more preferentially those of formulae (III) and (VII), may be added simultaneously to the internal mixer or external mixer, or to the reactor if the grafting is carried out in solution. They may also be added non-simultaneously with respect to one another, the order being immaterial for the grafting of these compounds onto the chain of the initial diene elastomer. After grafting, the diene elastomer has one or more pendant groups along its chain, which come from the reaction of grafting of the compounds of formulae (I) and (V) (or the preferred compounds mentioned above). Advantageously, these pendant groups are randomly distributed along the chain of the diene elastomer.

[0053] The molar degree of grafting of the compound of formula (I), preferably of formula (Ib), more preferentially of formula (III), is in the range of 0.01 to 5%, preferably of 0.01 to 1%, more preferentially of 0.1 to 1%, and the molar degree of grafting of the compound of formula (V), preferably of formula (Vb), more preferentially of formula (VII), is in the range of 0.01 to 5%, preferably of 0.01 to 1%, more preferentially of 0.1 to 1%.

[0054] According to a second embodiment of these compositions, the grafting of the diene elastomer with the compounds of formulae (I) and (V), preferably with the compounds of formulae (Ib) and (Vb), and even more preferentially with the compounds of formulae (III) and (VII), is carried out simultaneously with the preparation of the rubber composition. In this case, both the diene elastomer not yet grafted and the compounds of formulae (I) and (V) (or the preferred compounds) are introduced in a first "non-productive" stage. Preferentially, in this same non-productive stage, the reinforcing filler is subsequently added, so as not to cause side reactions with the compounds of formulae (I) and (V). Thus, according to a second embodiment of the process, the process comprises the following steps: during bulk compounding, mixing the compound of formula (I) as defined above, preferably the compound of formula (Ib), more preferentially the compound of formula (III), the compound of formula (V) as defined above, preferably the compound of formula (Vb), more preferentially the compound of formula (VII), into the diene elastomer, at a temperature in particular ranging from 60 to 140°C, in particular for a time ranging from 30 seconds to 3 minutes; under these temperature and time conditions, a grafting rate of preferably at least 60%, more preferentially at least 80%, is achieved, preferably followed by mixing the reinforcing filler, as well as all the basic constituents of the composition except the chemical crosslinking system, and kneading the combined mixture thermomechanically one or more times until a maximum temperature is reached in the range of 130 to 200°C, preferably 145 to 185°C; cooling the combination to a temperature below 100°C; followed by incorporating a chemical crosslinking system; kneading the combined mixture until the maximum temperature is not more than 120°C; and optionally The rubber composition thus obtained is then extruded or calendered. Advantageously, the steps of this second embodiment of the method are consecutive.

[0055] Semi-finished products for tires and tires Another subject of the invention is a semi-finished product made of rubber for tires, comprising the rubber composition of the invention as defined above. A semi-finished product is a product made of rubber intended for the manufacture of tires. It may be the tread, the underlayer, the crown reinforcing plies (for example working, protective or hooping plies), the carcass reinforcing plies, the sidewall plies, the bead plies, the protector plies, the underlayer plies, the rubber block plies and other plies that constitute the interface between the various parts of the tire. Preferably, the semi-finished product is a tread. Another subject of the invention is a tire, comprising at least one rubber composition according to the invention or comprising a semi-finished tire product as described above. The tire of the invention may be intended for equipping non-motorized vehicles, in particular bicycles, or industrial vehicles, such as agricultural heavy vehicles or earthmoving machines, selected from the following types of motorized vehicles: passenger cars, SUVs (sports utility vehicles), two-wheelers (in particular motorcycles), aircraft, vans, heavy vehicles (i.e. metro cars, buses, road heavy vehicles (trucks and trailers)), off-road vehicles, or other transport or transportation vehicles.

[0056] In addition to the subject matter described above, the present invention relates to at least one of the subject matters described in the following embodiments. 1. A rubber composition based on at least one diene elastomer, at least one reinforcing filler, at least one chemical crosslinking system and, optionally, at least one compound of formula (I) previously grafted to said diene elastomer: [ka] During the ceremony, A is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; E is a divalent hydrocarbon group, optionally containing one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom. Rubber composition. 2. The rubber composition according to claim 1, wherein the diene elastomer is selected from the group consisting of ethylene / propylene / diene monomer copolymer, butyl rubber, natural rubber, synthetic polyisoprene, polybutadiene, butadiene copolymer, isoprene copolymer, and mixtures of these elastomers. 3. The rubber composition according to embodiment 1 or 2, wherein the molar degree of grafting of the compounds of formula (I) is in the range of 0.01 to 5%, preferably 0.01 to 1%, more preferentially 0.1 to 1%. 4. The group A is a C6-C substituted, optionally with one or more identical or different, preferably linear or branched, aliphatic hydrocarbon chains. 14 The rubber composition according to any one of embodiments 1 to 3, wherein the hydrocarbon chain is an arenediyl ring, and is optionally substituted or interrupted by one or more heteroatoms. 5. A rubber composition in which the compound of formula (I) is selected from the compounds (Ia) and (Ib): [ka] During the ceremony, One group selected from R1 to R5 in formula (Ia) and one group selected from R1 to R7 in formula (Ib) represent a group of the following formula (II): [ka] (II) In the formula, E and X are as described in Example 1. The four groups selected from R1 to R5 of formula (Ia) other than the group of formula (II) and the six groups selected from R1 to R7 of formula (Ib) other than the group of formula (II) are identical or different and independently represent a hydrogen atom or, preferably, a saturated, linear or branched aliphatic hydrocarbon chain optionally substituted or interrupted by one or more heteroatoms. The rubber composition according to any one of the first to fourth embodiments. 6. The group E is preferably a saturated, linear or branched C-C alkyl group, optionally interrupted by one or more nitrogen, sulfur or oxygen atoms. 24 , and more preferentially C1-C10 6. The rubber composition according to claim 1, wherein the hydrocarbon chain is preferably a C1-C6 hydrocarbon chain, and more preferably a C1-C6 hydrocarbon chain. 7. The group E is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 7. The rubber composition according to any one of claims 1 to 6, wherein the alkylene is C1-C6 alkylene, more preferentially. 8. The rubber composition according to any one of embodiments 1 to 7, wherein the compound of formula (I) is a compound of formula (Ib). 9. The rubber composition according to any one of embodiments 1 to 8, wherein the compound of formula (I) is a compound of formula (III). [ka] (III) 10. A rubber composition additionally comprising at least one compound of formula (V) optionally pre-grafted to a diene elastomer: [ka] (V) During the ceremony, A1 is an arenediyl ring optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which are optionally substituted or interrupted by one or more heteroatoms; and E1 is a divalent hydrocarbon group optionally containing one or more heteroatoms The rubber composition according to any one of the first to ninth embodiments. 11. The rubber composition according to embodiment 10, wherein the molar degree of grafting of the compound of formula (V) is in the range of 0.01 to 5%, preferably 0.01 to 1%, more preferentially 0.1 to 1%. 12. The group A1 is a C6-C substituted, optionally with one or more identical or different, preferably linear or branched, aliphatic hydrocarbon chains. 14 12. The rubber composition according to claim 10 or 11, wherein the hydrocarbon chain is an arenediyl ring, and the hydrocarbon chain is optionally substituted or interrupted with one or more heteroatoms. 13. A rubber composition in which the compound of formula (V) is selected from compounds of formulae (Va) and (Vb): [ka] During the ceremony, R8 to R in formula (Va) 12 and R8 to R in formula (Vb): 14 One group selected from represents a group of formula (VI): [ka] (VI) E1 is as described in Example 10; and R8 to R in formula (Va) 12 four groups other than the group of formula (VI), and R to R of formula (Vb) 14 The six groups other than the one representing the group of formula (VI), selected from the following, are identical or different and are each independently a hydrogen atom or, preferably, a saturated, linear or branched aliphatic hydrocarbon chain, optionally substituted or interrupted by one or more heteroatoms. The rubber composition according to any one of embodiments 10 to 12. 14. The group E1 in the compound of formula (V) is Preferably, saturated, linear or branched C1-C optionally interrupted by one or more nitrogen, sulfur or oxygen atoms. 24 , preferably C1-C 10 14. The rubber composition according to any one of embodiments 10 to 13, wherein the C1-C6 hydrocarbon chain is more preferentially a C1-C6 hydrocarbon chain. 15. The group E1 of the compound of formula (V) is selected from the group consisting of -R- and -OR-, where R is a linear or branched C1-C 24 , preferably C1-C 10 15. The rubber composition according to any one of embodiments 10 to 14, wherein the alkylene is C1-C6 alkylene, more preferentially. 16. The rubber composition according to any one of embodiments 10 to 15, wherein the compound of formula (V) is a compound of formula (Vb). 17. The rubber composition according to any one of embodiments 10 to 17, wherein the compound of formula (V) is a compound of formula (VII). [ka] (VII) 18. The rubber composition according to any one of claims 1 to 17, wherein the reinforcing filler is carbon black or a carbon black mixture. 19. The rubber composition according to any one of the first to eighteenth embodiments, wherein the reinforcing filler is a reinforcing inorganic filler or a mixture of reinforcing inorganic fillers, preferably silica or a mixture of silicas. 20. The rubber composition according to any one of the first to 19th embodiments, wherein the reinforcing filler is a mixture of at least one carbon black and at least one reinforcing inorganic filler, preferably a mixture of at least one carbon black and at least one silica. 21. The rubber composition according to claim 19 or 20, wherein the composition additionally comprises a coupling agent for coupling the reinforcing inorganic filler and the diene elastomer. 22. The rubber composition of claim 21, wherein the coupling agent is selected from the group consisting of organosilane polysulfides, polyorganosiloxanes, mercaptosilanes, and blocked mercaptosilanes. 23. The rubber composition according to any one of embodiments 1 to 23, wherein the content of the reinforcing filler is in the range of 10 to 200 phr, preferably 30 to 180 phr, more preferentially 40 to 160 phr. 24. The rubber composition according to any one of claims 1 to 23, further comprising a plasticizer. 25. The rubber composition of claim 22, wherein the plasticizer is selected from the group consisting of plasticizing hydrocarbon resins having a Tg greater than 20° C., plasticizing oils, and mixtures thereof. 26. A semi-finished product made of rubber for tires, characterized in that it contains a rubber composition as defined in any one of claims 1 to 25. 27. A tire comprising at least one semi-finished product according to embodiment 26 or at least one composition according to any one of embodiments 1 to 25. EXAMPLES

[0057] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. 1 Tests and measurements used 1.1 Determination of glass transition temperature The glass transition temperature Tg of a polymer is measured using a differential calorimeter (differential scanning calorimeter) according to standard ASTM D3418 (2015).

[0058] 1.2 Determination of number average molecular weight (Mn), weight average molecular weight (Mw), and polydispersity index of elastomers Size Exclusion Chromatography (SEC) is used. SEC allows the separation of macromolecules in solution according to size through a column packed with a porous gel. The macromolecules are separated according to their hydrodynamic volume, with the largest eluting first. SEC is not an absolute method, but it allows the determination of the molar mass distribution of the elastomer. The various number average molecular weights (Mn) and weight average molecular weights (Mw) may be determined using commercially available standards, and the polydispersity index (PI=Mw / Mn) may be calculated by "Moore" calibration. Preparation of elastomer samples to be tested: No specific treatment is performed on the elastomer samples before analysis. The samples are dissolved directly in chloroform or in a mixture [tetrahydrofuran + 1% by volume diisopropylamine + 1% by volume triethylamine + 1% by volume distilled water (vol% = volume percentage)] at a concentration of approximately 1 g / L. The solution is then filtered through a filter with a pore size of 0.45 μm before injection. SEC analysis The equipment used is a Waters Alliance chromatograph. Depending on the solvent used to dissolve the elastomer, the elution solvent is a mixture [tetrahydrofuran + 1% by volume diisopropylamine + 1% by volume triethylamine] or chloroform. The flow rate is 0.7 mL / min, the system temperature is 35 °C, and the analysis time is 90 min. A set of four Waters columns in series (two Styragel HMW7, one Styragel HMW6E, and one Styragel HT6E) is used. The volume of the elastomer sample solution injected is 100 μL. The detector is a Waters 2410 differential refractometer with a wavelength of 810 nm. The software used to use the chromatographic data is the Waters Empower system. The calculated average molar masses are related to a calibration curve obtained from the commercially available PSS Ready Cal-Kit polystyrene standards.

[0059] 1.3 Molecular characterization Structural analysis and molar purity of the synthesized molecules are performed by NMR analysis. Spectra are obtained on a Bruker Avance 3400 MHz spectrometer equipped with a broadband 5 mm (BBFO) Z-axis gradient probe. Quantitative 1 H NMR experiments use a 30° single pulse sequence with 64 acquisitions and a repetition time of 3 seconds between each. Unless otherwise indicated, samples are dissolved in the deuterated solvent deuterated dimethyl sulfoxide (DMSO). A deuterated solvent is also used for the lock signal. For example, the signal of the deuterated DMSO protons at 2.44 ppm is calibrated against a 0 ppm TMS standard. 1 H NMR spectrum and 2D 1 H / 13 C HSQC and 1 H / 13 Combining this with C HMBC experiments allows the determination of the structure of the molecule (see assignment table). Molar quantification is achieved using quantitative 1D 1H NMR spectra. Mass spectrometry analysis is performed by direct infusion with electrospray ionization (DI / ESI). Analysis was performed on a Bruker HCT spectrometer (flow rate 600 μL / min, nebulizer gas pressure 68.95 kPa (10 psi), nebulizer gas flow rate 4 L / min).

[0060] 1.4 Preparation of compounds to be grafted onto diene elastomers The molar content of the compounds grafted onto the diene elastomer is determined by NMR analysis. The spectra are acquired on a Bruker 500 MHz spectrometer equipped with a Cryo probe with a 5 mm (BBFO) Z-axis gradient. Quantitative 1 H NMR experiments were performed using a 30° single pulse sequence with a repetition time of 5 seconds between each acquisition. To obtain the lock signal, samples were dissolved in deuterated chloroform (CDCl3). 2D NMR experiments confirmed the nature of the grafted units from the chemical shifts of carbon and proton atoms.

[0061] 1.5 Dynamic Characteristics Dynamic properties G* and tan(δ) max The viscosity is measured on a viscoanalyzer (Metravib VA4000) according to the standard ASTM D5992-96. A vulcanized composition sample (4 mm thick, 400 mm cross-sectional area) was subjected to an alternating single sinusoidal shear stress at a frequency of 10 Hz. 2 The response of the specimen (cylindrical specimen) is recorded according to standard ASTM D1349-09 under reference temperature conditions (23°C). Strain amplitude sweeps are performed from 0.1 to 50% peak-to-peak (outward cycle) and then from 50 to 0.1% peak-to-peak (return cycle). The results used are the complex dynamic shear modulus G* at 23°C and the dynamic loss factor tan(δ) at 23°C. For the outward cycle, the value of the complex dynamic shear modulus G* at 50% strain (G* 50%外向き ) is recorded at 23°C. In the return cycle, the maximum dynamic loss factor tan(δ) observed (tan(δ) max ) is recorded at 23°C. The tan(δ) at 23°C of the various test samples max and G* at 23°C 50%外向きis calculated and for subsequent comparison, the results are expressed as a standard of 100, with an arbitrary value of 100 as the control. Tan(δ) at 23°C max Calculate the value of the test sample based on 100 according to the procedure: (tan (δ) of the test sample at 23 ° C.) max Value / tan(δ) of control at 23°C max value) x 100. A result less than 100 indicates reduced hysteresis and a corresponding improvement in rolling resistance performance. G* at 23°C 50%外向き Calculate the value of the test sample based on 100 according to the procedure: (G* at 23 ° C of the test sample) 50%外向き Value / G* at 23°C of control 50%外向き value) × 100. If the result is greater than 100, the complex dynamic shear modulus G* at 50% strain at 23°C 50%外向き and a corresponding increase in material stiffness are shown.

[0062] 2. Synthesis of Compounds 2.1 Synthesis of compound A: 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide [ka] 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide is synthesized in six steps, designated step a1, step a2, step b1, step b2, step c, and step d. Step a1 is carried out according to procedure 1, step a2 according to procedure 2, and step b1 according to procedure 3. Steps b2 and c are carried out according to procedure 4. Step d is carried out according to procedure 5. Step a1: Preparation of 2-hydroxy-1-naphthaldehyde [ka]

[0063] Step 1: This compound may be obtained by formylation from naphthol according to the "Reimer-Tiemann" procedure described by Russell, Alfred and Lockhart, Luther B. in Organic Syntheses, 22, 63-4; 1942, or by Wynberg, Hans and Meijer, Egbert W. in Organic Reactions (Hoboken, NJ, USA), 28, 1982, or by the procedure described by Casiraghi, Giovanni et al. in the Journal of the Chemical Society, Perkin Transactions 1: Organic and Bio-Organic Chemistry (1972-1999), (9), 1862-5, 1980, or by the Vilsmeier reaction described by Jones, Gurnos and Stanforth, Stephen P. in Organic Reactions (Hoboken, NJ, USA), 49, 1997. 2-Hydroxy-1-naphthaldehyde is commercially available and may be obtained, for example, from Aldrich (CAS708-06-5). Step a2: Preparation of 1-(2-chloroethyl)imidazolidin-2-one [ka]

[0064] Step 2: This compound may be obtained according to the procedures described in WO 2012 / 007684. Step b1: Preparation of 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde [ka]

[0065] Step 3: A mixture of 2-hydroxy-1-naphthaldehyde (20.0 g, 0.116 mol), potassium carbonate (24.08 g, 0.174 mol) and 1-(2-chloroethyl)imidazolidin-2-one (25.9 g, 0.174 mol) in DMF (20 mL) is heated at 75 ° C (bath temperature) for 3.0-3.5 h. Subsequently, a second portion of 1-(2-chloroethyl)imidazolidin-2-one (17.26 g, 0.116 mol) is added and the reaction medium is stirred at 75 ° C (bath temperature) for 9-10 h. When the temperature has decreased to 40-45 ° C, the reaction medium is poured into a solution of sodium hydroxide (10 g, 0.25 mol) in water (700 mL). The mixture is stirred for 10-15 min. The precipitate is filtered off and washed on the filter with distilled water (3 times with 400 mL). A grey solid (31.51 g, 95% yield) was obtained with a molar purity of 85% ( 1 H NMR). [ka] [Table 1] Solvent: CDCl3 Steps b2 and c: Preparation of 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde oxime [ka] The product isolated at the end of step 3 is used in step 4.

[0066] Step 4: A solution of hydroxylamine (2.05 g, 31.0 mmol, 50% in water, Aldrich) in ethanol (5 mL) is added to a solution of 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde (6.3 g, 22.2 mmol) in ethanol (30 mL) at 45° C. (bath temperature). The reaction medium is stirred at 55° C. (bath temperature) for 4 hours. When the temperature has decreased to 40° C., ethyl acetate (30 mL) is added dropwise over 15 minutes. The precipitate is filtered off and washed on the filter with an ethanol / ethyl acetate mixture. A white solid (4.00 g, 60% yield) is obtained. The molar purity ( 1 H NMR) is greater than 95%. [ka] [Table 2] Solvent: MeOH Step d: Preparation of 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide [ka]

[0067] Step 5: An aqueous solution of NaOCl (74.44 g / L; 98 mL; 4.0 eq.) (eq. = molar equivalents) is added dropwise over 10 minutes to a suspension of the above 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde oxime (7.30 g; 24.4 mmol) in ethyl acetate (230 mL) cooled to 1 ° C (bath temperature = 0 ° C). The reaction medium is stirred for 8.5 hours at 0-2 ° C (bath temperature = 0 ° C). A second portion of an aqueous solution of NaOCl (74.44 g / L; 98 mL; 4.0 eq.) is added over 5 minutes. The reaction medium is stirred for 10-11 hours at 0-2 ° C (bath temperature = 0 ° C). The precipitate is filtered off and washed on the filter with water (2 times with 25 mL) and then with ethyl acetate (2 times with 10 mL). This gives a white solid with a melting point of 127.0-127.5 °C (6.24 g; 18.7 mmol; 77% yield). Compound A, 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, is obtained with a molar purity of >92% ( 1 H NMR), less than 6 mol % 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, and 2 mol % residual solvent impurities. [ka] [Table 3] Solvent: CDCl3

[0068] 2.2 Synthesis of compound B: 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide Repeat steps 1 to 4 in section 2.1 to obtain 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde oxime, then carry out step 6 described below to obtain 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide.

[0069] Step 6: Aqueous NaOCl (78 g / L; 35 mL; 1.46 eq.) is added dropwise over 15 min to a solution of 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthaldehyde oxime (7.5 g; 25.06 mmol) in dichloromethane (300 mL) cooled to 4 ° C (bath temperature = 0 ° C). The reaction medium is stirred for 60-70 min at 4-5 ° C. The organic phase is separated. The aqueous phase is extracted with dichloromethane (25 mL). The combined organic solutions are washed with water (2 times with 25 mL). The solvent is evaporated under reduced pressure to 40-50 mL. 40 / 60 petroleum ether (60 mL) is added and allowed to crystallize. The precipitate is filtered off and washed with 40 / 60 petroleum ether (2 times with 30 mL). A white solid (6.46 g, 87% yield) is obtained. 1 Product B is obtained with a molar purity of >99% as estimated by H NMR and <1% residual solvent impurities. [ka] [Table 4] Solvent: CDCl3

[0070] 3. Implementation of modified polymers 3.1 Styrene / butadiene copolymer grafted with 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide Compound A, 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide (0.27 g; 0.81 mmol), obtained by the synthesis method described in section 2.1, is mixed in an open mill (external mixer, 23° C.) with 20 g of non-functionalized styrene / butadiene copolymer (containing 26.5% by weight of styrene relative to the total weight of the polymer and 25% by weight of 1,2-butadiene units relative to the weight of the butadiene part; Mn=150,000 g / mol, PI=1.84, measured according to the method described in section 1.2). The mixture is homogenized by 15 tumblings. This compounding step is followed by a heat press treatment at 120° C. for 10 minutes under a pressure of 10 bar. 1Analysis by H NMR demonstrated a molar degree of grafting of 0.29% and a molar grafting rate of 96%. Chemical shifts that allow the determination of the degree of grafting: 7.6~8.2ppm:6 aromatic H 4.2~4.3ppm: 2H CH2-O 3.1~3.8ppm:6H CH2-N

[0071] 3.2 Polyisoprene grafted with 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide Compound A, 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide (0.29 g; 0.88 mmol), obtained by the synthesis method described in section 1.2, is mixed in an open mill (external mixer, 23° C.) with 20 g of synthetic polyisoprene (containing 99.35% by weight of cis-1,4-isoprene units and 0.65% by weight of 3,4-isoprene units; Mn=375,000 g / mol, PI=3.6, measured according to the method described in section 1.2). The mixture is homogenized by 15 inversions. This compounding step is followed by a heat press treatment at 120° C. for 10 minutes under a pressure of 10 bar. 1 Analysis by H NMR allowed us to demonstrate a molar degree of grafting of 0.2% and a molar grafting rate of 66%. Chemical shifts that allow the determination of the degree of grafting: 7.6~8.2ppm:6 aromatic H 4.2~4.3ppm: 2H CH2-O 3.1~3.8ppm:6H CH2-N

[0072] 4. Examples of Rubber Compositions 4.1 Example 1 The purpose of this test is to demonstrate the improved performance of rubber properties in the compositions of the present invention compared to conventional non-compatible compositions that do not contain modified elastomers and to prior art compositions that do contain modified elastomers. In particular, these compositions are defined as follows: The non-compatible composition C1 is a "conventional" rubber composition used as a tire tread, specifically comprising non-grafted synthetic polyisoprene, silica, and a silane polysulfide coupling agent; Incompatible composition C2 is identical to composition C1 except that it additionally contains compound B grafted to the synthetic polyisoprene; Composition C3 according to the invention is a composition identical to composition C1, except that it additionally comprises compound A which is grafted to the synthetic polyisoprene. The contents of the various components of these compositions, expressed in phr (parts by weight per 100 parts by weight of elastomer), are given in Table 1. [Table 5] Compositions C2 and C3 contain the same number of moles of grafted compound A or B, ie 0.2 mol %. (1) Polyisoprene containing 99.35% by weight of cis-1,4-isoprene units and 0.65% by weight of 3,4-isoprene units; Mn=375,000 g / mol, PI=3.6, determined according to the method described in 1.2; (2) Compound B: 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, synthesized according to the method described in section 2.2; (3) Compound A: 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, synthesized according to the method described in section 2.1; (4) Silica, Zeosil 1165MP, available from Solvay; (5) Bis[3-(triethoxysilyl)propyl]tetrasulfide (TESPT), sold by Evonik under the name Si69; (6) N234 grade carbon black, available from Cabot Corporation; (7) N-(1,3-dimethylbutyl)-N'-phenyl-para-phenylenediamine, sold by Flexsys under the name Santoflex6-PPD; (8) 2,2,4-trimethyl-1,2-dihydroquinoline, sold by Flexsys; (9) Zinc oxide (industrial grade), sold by Umicore; (10) Stearin, Pristerene 4031, sold by Uniqema; (11) N-Cyclohexyl-2-benzothiazole sulfenamide, sold by Flexsys under the name Santocure CBS.

[0073] Compositions C1 to C3 are prepared as follows: 85 cm of diene elastomer are added to 3 The mixture is then charged into a Polylab internal mixer at 100° C. and filled to 70%. The initial container temperature is about 110° C. For the compositions related to compound A or compound B, compound A or compound B is charged simultaneously with the diene elastomer. A thermomechanical work is then carried out at 120° C. for 1.5 minutes. Then, for each of compositions C1 to C3, one or more reinforcing fillers, a coupling agent for the fillers and the diene elastomer are charged, followed by mixing for 1 to 2 minutes, followed by the charging of the various other components, except the vulcanization system. A thermomechanical work (non-productive phase) is then carried out until a maximum drop temperature of 160° C. is reached, in steps lasting a total of about 5 minutes. After recovering and cooling the mixture thus obtained, the vulcanization system (sulfur and sulfenamide accelerators) is added in an external mixer (homofinisher) at 25° C., and the combination is mixed for about 5 to 6 minutes (productive phase). The composition thus obtained is then calendered into rubber plaques (2 to 3 mm thick) or sheets for the measurement of physical or mechanical properties. The rubber properties of these compositions are measured after curing for 60 minutes at 150° C. The results obtained are shown in Table 2. [Table 6] As expected from Table 2, the non-compatible composition C2, which includes an elastomer modified with a compound containing unsubstituted imidazolidinone functionality, exhibits a significantly lower hysteresis (tan(δ) at 23° C.) than the non-compatible composition C1, which does not include a modified elastomer. max) is seen to show a reduction in rolling resistance. Surprisingly, the composition C3 of the present invention comprising an elastomer modified with a compound comprising an N-substituted imidazolidinone functional group shows a significant reduction in hysteresis compared to the non-compatible composition C1, and also compared to the non-compatible composition C2, which already showed good hysteresis properties compared to the non-compatible composition C1. Thus, the elastomers modified with the compounds used in the context of the present invention can provide a reduction in hysteresis of compositions comprising them, thereby improving the rolling resistance performance of these compositions.

[0074] 4.2 Implementation 2 The purpose of this test is to demonstrate the improved rubber properties of certain compositions of the present invention compared to conventional non-compatible compositions that do not contain modified elastomers and to non-compatible compositions of the prior art that do contain modified elastomers. In particular, these compositions are defined as follows: Non-conforming composition C4 is a "conventional" rubber composition used as a tire tread, specifically including non-grafted styrene / butadiene copolymer (SBR), silica, and a silane polysulfide coupling agent; Non-compatible composition C5 is identical to composition C4 except that it additionally contains compound B grafted to the SBR; Composition C6 according to the invention is a composition identical to composition C5, but additionally comprising compounds A and B grafted to SBR; Non-compliant composition C7 is identical to composition C4 except that it contains synthetic polyisoprene instead of SBR; Non-compatible composition C8 is identical to composition C7 except that it additionally contains compound B grafted to the synthetic polyisoprene; Composition C9 according to the invention is the same composition as composition C7, except that it additionally comprises compounds A and B which are grafted to the synthetic polyisoprene. The contents of the various components of these compositions, expressed in phr (parts by weight per 100 parts by weight of elastomer), are given in Table 3. [Table 7] (1) Polyisoprene containing 99.35% by weight of cis-1,4-isoprene units and 0.65% by weight of 3,4-isoprene units; Mn=375,000 g / mol, PI=3.6, determined according to the method described in 1.2; (2) a non-functionalized styrene / butadiene copolymer containing 26.5% by weight of styrene, relative to the total weight of the copolymer, and 25% by weight of 1,2-butadiene units, relative to the weight of the butadiene part; Mn=150,000 g / mol, PI=1.84, determined according to the method described in section 1.2; (3) Compound B: 2-(2-(2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, synthesized according to the method described in section 2.2; (4) Compound A: 2-(2-(3-chloro-2-oxoimidazolidin-1-yl)ethoxy)-1-naphthonitrile oxide, synthesized according to the method described in section 2.1; (5) Silica, Zeosil 1165MP, available from Solvay; (6) Bis[3-(triethoxysilyl)propyl]tetrasulfide (TESPT), sold by Evonik under the name Si69; (7) N234 grade carbon black, available from Cabot Corporation; (8) N-(1,3-dimethylbutyl)-N'-phenyl-para-phenylenediamine, sold by Flexsys under the name Santoflex6-PPD; (9) 2,2,4-trimethyl-1,2-dihydroquinoline, sold by Flexsys; (10) Zinc oxide (industrial grade), sold by Umicore; (11) Stearin, Pristerene 4031, sold by Uniqema; (12) N-Cyclohexyl-2-benzothiazole sulfenamide, sold by Flexsys under the name Santocure CBS.

[0075] The composition is prepared as follows: 85 cm of diene elastomer is added. 3The mixture is then charged into a Polylab internal mixer at 100° C. and filled to 70%. The initial container temperature is about 110° C. For the compositions related to compound B or compound A, compound B or compounds A and B are charged simultaneously with the diene elastomer. A thermomechanical operation is then carried out at 120° C. for 1.5 minutes. Then, for each of compositions C4 to C9, one or more reinforcing fillers, a coupling agent for the fillers and the diene elastomer are charged, followed by mixing for 1 to 2 minutes, followed by the charging of the various other components, except the vulcanization system. A thermomechanical operation (non-productive phase) is then carried out until a maximum drop temperature of 160° C. is reached, in steps lasting a total of about 5 minutes. After recovering and cooling the mixture thus obtained, the vulcanization system (sulfur and sulfenamide accelerators) is added in an external mixer (homofinisher) at 25° C., and the combination is mixed for about 5 to 6 minutes (productive phase). The composition thus obtained is then calendered into rubber plaques (2 to 3 mm thick) or sheets for the measurement of physical or mechanical properties. The rubber properties of these compositions are measured after curing for 60 minutes at 150° C. The results obtained are shown in Table 4. [Table 8] From Table 4, as expected, the non-compatible compositions C5 and C8, which contain elastomers grafted with compounds containing unsubstituted imidazolidinone functional groups, have the same stiffness (G* at 23° C.) as the non-compatible compositions C4 and C7, which do not contain modified elastomers, respectively. 50%外向き) shows a reduction in hysteresis. Surprisingly, the composition C6 according to the invention, comprising an elastomer modified with a compound containing an N-substituted imidazolidinone functional group and a compound containing an unsubstituted imidazolidinone functional group, shows a significant reduction in hysteresis compared to the non-compatible composition C5, which already showed a reduction in hysteresis compared to the non-compatible composition C4. This reduction in hysteresis occurs without a reduction in the stiffness properties after curing, which is surprising, since it is known to those skilled in the art that hysteresis and stiffness properties after curing are two opposing properties of rubber compositions. It is known that improving stiffness properties before curing leads to a worsening of hysteresis and vice versa. However, here we observe a significant improvement in the stiffness / hysteresis tradeoff after curing for the composition C6 according to the invention, compared to the non-compatible compositions C4 and C5. This same result is observed for the composition C9 according to the invention, compared to the non-compatible compositions C7 and C8, even though the stiffness before curing is lower for the composition C9 according to the invention, compared to the non-compatible composition C8. This reduction in stiffness before curing is still very small considering the large reduction in hysteresis of composition C9 according to the invention.

Claims

1. at least one diene elastomer, at least one reinforcing filler, At least one chemical crosslinking system, and at least one compound of formula (I), optionally previously grafted onto said diene elastomer, A rubber composition based on: [Formula 1] During the ceremony, A is an arenediyl ring, which may be optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which may be optionally substituted or interrupted with one or more heteroatoms; E is a divalent hydrocarbon group, which may optionally contain one or more heteroatoms; and X represents a halogen atom, preferably a chlorine atom. The molar content of the compound of formula (I) in the rubber composition is in the range of 0.1 mol% to 5 mol%, mol% meaning the units of the compound of formula (I) present in the rubber composition per 100 units of diene elastomer of the rubber composition, expressed as a molar percentage. Rubber composition.

2. 2. The rubber composition of claim 1, wherein the diene elastomer is selected from the group consisting of ethylene / propylene / diene monomer copolymers, butyl rubber, natural rubber, synthetic polyisoprene, polybutadiene, butadiene copolymers, isoprene copolymers, and mixtures of these elastomers.

3. A rubber composition in which the compound of formula (I) is selected from compounds (Ia) and (Ib): [Case 2] During the ceremony, R in the formula (Ia) 1 ~R 5and R of formula (Ib) 1 ~R 7 One group selected from represents a group of formula (II): [C3] (II) wherein E and X are as defined in claim 1; and R in the formula (Ia) 1 ~R 5 and R 1 ~R 7 are identical or different and independently represent a hydrogen atom or a preferably saturated, linear or branched aliphatic hydrocarbon chain, which may be optionally substituted or interrupted by one or more heteroatoms; The rubber composition according to claim 1 or 2.

4. The E is preferably a saturated, linear or branched C 1 -C 24 , with higher priority given to C 1 -C 10 , and more preferentially C 1 -C 6 The rubber composition according to any one of claims 1 to 3, wherein the aliphatic hydrocarbon chain is optionally interrupted by one or more nitrogen, sulfur or oxygen atoms.

5. The rubber composition according to claim 3 or 4, wherein the compound of formula (I) is a compound of formula (Ib).

6. The rubber composition according to any one of claims 1 to 5, wherein the compound of formula (I) is a compound of formula (III). [C4] (III)

7. A rubber composition additionally comprising at least one compound of formula (V), optionally previously grafted to said diene elastomer: [C5] (V) During the ceremony, A 1 is an arenediyl ring, which may be optionally substituted with one or more identical or different, preferably saturated, linear or branched, aliphatic hydrocarbon chains, which may be optionally substituted or interrupted with one or more heteroatoms; and E 1 is a divalent hydrocarbon group that may optionally contain one or more heteroatoms The rubber composition according to any one of claims 1 to 6.

8. A rubber composition, wherein the compound of formula (V) is selected from compounds of formulas (Va) and (Vb): [C6] During the ceremony, R in the formula (Va) 8 ~R 12 and R in formula (Vb) 8 ~R 14 One group selected from represents a group of formula (VI): [C7] (VI) E 1 is as claimed in claim 7; and R in the formula (Va) 8 ~R 12 and R 8 ~R 14 are identical or different and independently represent a hydrogen atom or a preferably saturated, linear or branched aliphatic hydrocarbon chain, which may be optionally substituted or interrupted by one or more heteroatoms; The rubber composition according to claim 7.

9. E of the compound of formula (V) 1 but preferably saturated, linear or branched C 1 -C 24 , preferably C 1 -C 10 , with higher priority given to C 1 -C 6 9. The rubber composition according to claim 7 or 8, which is a hydrocarbon chain, said aliphatic hydrocarbon chain optionally being substituted or interrupted by one or more heteroatoms.

10. The rubber composition according to claim 8 or 9, wherein the compound of formula (V) is a compound of formula (Vb).

11. The rubber composition according to any one of claims 7 to 10, wherein the compound of formula (V) is a compound of formula (VII). [C8] (VII)

12. The rubber composition according to any one of claims 1 to 11, wherein the reinforcing filler is selected from carbon black, reinforcing inorganic fillers, and mixtures of carbon black and inorganic fillers.

13. The rubber composition according to any one of claims 1 to 12, additionally comprising a plasticizer.

14. Semi-finished product made of rubber for tires, characterized in that it comprises at least one rubber composition according to any one of claims 1 to 13.

15. A tire, characterized in that it comprises at least one semi-finished product according to claim 14 or at least one composition according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • A rubber composition containing a modified elastomer, a method for producing the rubber composition, and a tire containing the rubber composition.

    JP2013531726A

  • A rubber composition comprising a diene elastomer having imidazole functional groups randomly distributed along the chain.

    JP2016535807A

  • Rubber composition containing 1,3-dipolar compound additive with imidazole functionality

    JP2017501240A

  • Composition on the basis of at least one specific polyaromatic compound

    WO2019007883A1

  • Polymer carrying specific pendant imidazolidinone functional groups

    WO2019007884A1