Thermoplastic resins, dihydrogenated plastic compounds

A thermoplastic resin with specific structural units and dihydroxy compounds addresses the need for improved heat resistance and optical properties in optical films, enhancing mechanical stability and productivity in display manufacturing.

JP7552158B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020147040
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-01
Publication Date
2024-09-18
Estimated Expiration
2040-09-01

AI Technical Summary

Technical Problem

There is a need for materials with improved heat resistance, optical properties, and mechanical properties in optical films used in displays, particularly during assembly processes and in high temperature and high humidity environments, while also requiring cost reductions and improved productivity in processes like film formation, stretching, and lamination.

Method used

A thermoplastic resin containing specific structural units represented by formulas (1), (2), and (3), along with dihydroxy compounds such as myo-inositol derivatives, which enhance heat resistance, mechanical properties, and optical properties, and are derived from biomass resources.

Benefits of technology

The resin achieves excellent heat resistance, mechanical properties, low water absorption, and optical properties, ensuring stability in varying environments and improving productivity in film production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552158000083
    Figure 0007552158000083
  • Figure 0007552158000076
    Figure 0007552158000076
  • Figure 0007552158000084
    Figure 0007552158000084
Patent Text Reader

Abstract

To provide a new thermoplastic resin, and a new dihydroxy compound used in production of the thermoplastic resin.SOLUTION: A thermoplastic resin includes a structural unit A represented by the following formula (1) in the molecule. In the formula (1), X represents a structure represented by formula (2) or formula (3).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel thermoplastic resin and a dihydroxy compound. [Background technology]

[0002] In recent years, there has been an increasing demand for transparent resins used in optical applications such as optical lenses, optical films, optical recording media, etc. In particular, the spread of thin flat panel displays (FPDs) such as liquid crystal displays and organic electroluminescence displays has been remarkable, and various optical films have been developed and used to improve display quality, such as by improving contrast and color, widening the viewing angle, and preventing external light reflection.

[0003] For example, in organic EL displays, a quarter-wave plate is used to prevent reflection of external light. A retardation film used in a quarter-wave plate is required to have a wide-band wavelength dispersion characteristic that can obtain ideal retardation characteristics at each wavelength in the visible range in order to suppress coloring and enable a clean black display. As an equivalent to this, for example, a retardation film that is made of a polycarbonate copolymer containing a bisphenol structure having a fluorene ring in the side chain and shows reverse wavelength dispersion in which the retardation becomes smaller as the wavelength becomes shorter (for example, see Patent Documents 1 and 2).

[0004] In addition, while conventional polycarbonate resins have mainly used bisphenol A as a monomer, in recent years, polycarbonate resins using isosorbide (ISB) as a monomer component have been developed. Polycarbonate resins using ISB have excellent properties such as heat resistance and optical properties, and their use in optical applications such as retardation films and as a replacement for glass is being considered (see, for example, Patent Documents 3 and 4). In addition, ISB is a dihydroxy compound obtained from biomass resources, and is also attracting interest as a carbon-neutral material that does not contribute to an increase in carbon dioxide emissions even when incinerated.

[0005] Inositol is a cyclic polyhydric alcohol obtained from biomass resources, and it is expected that it can be used to form a polymer by linking it with a compound that reacts with a hydroxyl group. Non-Patent Documents 1 to 4 report that polyurethane was synthesized from an inositol derivative and showed improved heat resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3325560 [Patent Document 2] Patent No. 5119250 [Patent Document 3] Patent No. 5346449 [Patent Document 4] JP 2012-214666 A [Non-patent literature]

[0007] [Non-Patent Document 1] "Journal of Polymer Science", Part A 51.3956, 2013 [Non-Patent Document 2] Atsushi Sudo, Yoshiya Shibata, Ayano Miyamoto, Yuka Tateoka, "Synthesis of polymers with fused ring systems in the main chain using myo-inositol as a raw material", Proceedings of the Society of Polymer Science, Japan, Society of Polymer Science, 2013, Vol. 62, No. 1, p. 396 [Non-Patent Document 3] Shuhei Okiyo, Atsushi Sudo, "Synthesis of network polyurethane using myo-inositol as a raw material", Proceedings of the Society of Polymer Science, Japan, Society of Polymer Science, 2013, Vol. 62, No. 1, p. 397 [Non-Patent Document 4] Taichi Sano, Masato Harada, Atsushi Sudo, "Regioselective urethanization of myo-inositol to give tetraol and synthesis of network polyurethane using this monomer," Proceedings of the Society of Polymer Science, Japan, Society of Polymer Science, 2013, Vol. 62, No. 1, p. 398 Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, in the use of optical films including retardation films, there is a demand for improving the heat resistance of materials so that the optical properties and dimensions of the film do not change in processes involving heating during the assembly process of polarizing plates and displays, and in high-temperature and high-humidity environments. In addition, there are demands for further improvement of optical properties and quality, cost reduction, and improvement of productivity in each process such as film formation, stretching, and lamination, and in order to meet these demands, materials that combine various excellent properties are desired. Specifically, there is a demand for improving heat resistance by improving the glass transition temperature, and for developing materials that have a high level of balance of physical properties such as optical properties such as wavelength dispersion of retardation and photoelastic coefficient, mechanical properties such as film toughness, and melt processability. There is a demand for the development of new materials that are excellent in such various physical properties.

[0009] The present invention has been made in view of the above background, and aims to provide a novel thermoplastic resin and a novel dihydroxy compound for use in producing the thermoplastic resin. [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that a thermoplastic resin containing a specific structure has excellent physical properties such as heat resistance, mechanical properties, optical properties, low water absorption, and moist heat resistance, and have arrived at the present invention.

[0011] [1] A thermoplastic resin containing a structural unit A represented by the following formula (1) in the molecule, wherein X in the formula (1) is a structure represented by the following formula (2) or (3): [ka] [ka] [ka]

[0012] In the formula (2), R 1 represents a hydrogen atom or an organic group, R 2 represents a direct bond or a divalent organic group, and in the formula (3), R 3 , R 4 each independently represents a hydrogen atom or an organic group, Z represents a divalent organic group, and * in the formulas (2) and (3) represents a bonding site.

[0013] [2] The thermoplastic resin according to [1], wherein X in the formula (1) is a structure represented by the formula (3). [3] The thermoplastic resin according to [1] or [2], wherein, in formula (3), Z is a divalent hydrocarbon group. [4] The thermoplastic resin according to any one of [1] to [3], wherein in the formula (3), Z is a divalent hydrocarbon group having 1 to 6 carbon atoms.

[0014] [5] In the formula (3), R 3 , R 4 are each independently a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. [6] The thermoplastic resin according to any one of [1] to [5], wherein the formula (3) is the following formula (4) or the following formula (5): [ka] [ka]

[0015] In the formulas (4) and (5), * indicates a binding site.

[0016] [7] The thermoplastic resin according to any one of [1] to [6], having a glass transition temperature of 100°C or higher and 200°C or lower. [8] The thermoplastic resin according to any one of [1] to [7], containing 1 wt % or more and 99 wt % or less of the structural unit represented by formula (1), when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt %. [9] The thermoplastic resin according to any one of [1] to [8], further comprising a structural unit derived from at least one dihydroxy compound selected from the group consisting of an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, a heteroalicyclic dihydroxy compound, and an aromatic dihydroxy compound.

[0017]

[10] The thermoplastic resin according to [9], containing 1 wt % or more and 95 wt % or less of structural units (excluding the structural unit A) derived from at least one dihydroxy compound selected from the group consisting of the aliphatic dihydroxy compound, the alicyclic dihydroxy compound, and the heteroalicyclic dihydroxy compound, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt %.

[11] The thermoplastic resin according to [9] or

[10] , which contains at least one of a structural unit derived from the alicyclic dihydroxy compound and a structural unit derived from the heteroalicyclic dihydroxy compound, and a structural unit represented by the formula (1).

[0018]

[12] The thermoplastic resin according to any one of [1] to

[11] , further comprising a structural unit derived from at least one dicarboxylic acid compound selected from the group consisting of an aliphatic dicarboxylic acid compound, an alicyclic dicarboxylic acid compound, a heteroalicyclic dicarboxylic acid compound, and an aromatic dicarboxylic acid compound.

[13] The thermoplastic resin according to any one of [1] to

[12] , containing 1 wt % or more and 95 wt % or less of a structural unit represented by the following formula (6), when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt %: [ka]

[0019]

[14] The thermoplastic resin according to any one of [1] to

[13] , containing 1 wt % or more and 95 wt % or less of a structural unit represented by the following formula (7), when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt %. [ka] In the formula (7), R 21 ~R 24 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.

[0020]

[15] The thermoplastic resin according to any one of [1] to

[14] , containing at least one structural unit selected from the following formulas (8) to (10) in an amount of 1 wt % or more and 70 wt % or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt %: [ka]

[0021] In the formula (8), R 5 ~R 8 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 6 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; X represents a substituted or unsubstituted alkylene group having 2 to 10 carbon atoms, a substituted or unsubstituted cycloalkylene group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms; and m and n each independently represent an integer of 0 to 5.

[0022] [ka]

[0023] [ka] In the formula (9) and the formula (10), R 9 ~R 11 each independently represents a direct bond or an alkylene group having 1 to 4 carbon atoms which may have a substituent, R 12 ~R 17 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an aryl group having 4 to 10 carbon atoms which may have a substituent, an acyl group having 1 to 10 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an aryloxy group having 1 to 10 carbon atoms which may have a substituent, an acyloxy group having 1 to 10 carbon atoms which may have a substituent, an amino group which may have a substituent, a vinyl group having 1 to 10 carbon atoms which may have a substituent, an ethynyl group having 1 to 10 carbon atoms which may have a substituent, a sulfur atom which has a substituent, a silicon atom which has a substituent, a halogen atom, a nitro group, or a cyano group, provided that R 12 ~R 17 At least two adjacent groups among these may be bonded to each other to form a ring.

[0024]

[16] The thermoplastic resin according to any one of [1] to

[15] , which is a polycarbonate or a polyester carbonate.

[0025]

[17] A dihydroxy compound represented by the following formula (11): [ka] In the formula (11), R 1 represents a hydrogen atom or an organic group, R 2 represents a direct bond or a divalent organic group.

[0026]

[18] A dihydroxy compound represented by the following formula (12): [ka] In the formula (12), R 3 , R 4 each independently represents a hydrogen atom or an organic group, and Z represents a divalent organic group.

[0027]

[19] The dihydroxy compound according to

[18] , wherein, in the formula (12), Z is a divalent hydrocarbon group.

[20] The dihydroxy compound according to

[19] , wherein in the formula (12), Z is a divalent hydrocarbon group having 1 to 6 carbon atoms.

[21] In the formula (12), R 3 , R 4 are each independently a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms.

[0028]

[22] The dihydroxy compound according to any one of

[18] to

[21] , wherein the formula (12) is the following formula (13) or the following formula (14): [ka] [ka] Effect of the Invention

[0029] According to the present invention, it is possible to provide a novel thermoplastic resin and a novel dihydroxy compound used for producing the thermoplastic resin. The thermoplastic resin has excellent physical properties such as heat resistance, mechanical properties, low water absorption, moist heat resistance, and optical properties. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is an NMR spectrum of the thermoplastic resin of Example 1. [Diagram 2] FIG. 2 is an NMR spectrum of the thermoplastic resin of Example 2. [Diagram 3] FIG. 3 is an NMR spectrum of the thermoplastic resin of Example 6. [Figure 4] FIG. 4 is an NMR spectrum of the thermoplastic resin of Example 10. [Diagram 5]FIG. 5 is an NMR spectrum of the thermoplastic resin of Example 11. [Figure 6] FIG. 6 is an NMR spectrum of the thermoplastic resin of Example 12. [Figure 7] FIG. 7 is an NMR spectrum of the thermoplastic resin of Example 13. [Figure 8] FIG. 8 is an NMR spectrum of the thermoplastic resin of Example 14. [Figure 9] FIG. 9 is an NMR spectrum of the thermoplastic resin of Example 15. [Figure 10] FIG. 10 is an NMR spectrum of the thermoplastic resin of Example 16. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The following describes in detail an embodiment of the present invention. The description of the components described below is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention.

[0032] In this specification, the term "structural unit" refers to a partial structure sandwiched between adjacent linking groups in a polymer, and a partial structure sandwiched between a polymerization reactive group present at the end of a polymer and a linking group adjacent to the polymerization reactive group. Also, the term "repeating structural unit" refers to a partial structure consisting of a structural unit and one adjacent linking group. For example, in the carbonate-based resin described below, the linking group is a carbonyl group.

[0033] In addition, in this specification, the number of carbon atoms of various substituents refers to the total number of carbon atoms including the number of carbon atoms of the substituents when the substituents further have substituents. In this specification, unless otherwise specified, "% by weight" and "% by mass" have the same meaning.

[0034] [Carbonate resin] (Structural unit A) The thermoplastic resin contains at least a structural unit represented by the following formula (1) (suitably referred to as structural unit A). The thermoplastic resin preferably has a repeating structural unit represented by formula (1'). In this case, the thermoplastic resin is a resin having a carbonate bond. In this specification, a thermoplastic resin having a carbonate bond is suitably referred to as a "carbonate-based resin". Examples of carbonate-based resins include polycarbonate resins having a carbonate bond, polyester carbonate resins having a carbonate bond and an ester bond, and the like. The thermoplastic resin in this specification is not particularly limited, but is, for example, a carbonate-based resin.

[0035] [ka]

[0036] [ka]

[0037] X in the formula (1) represents a structure represented by the following formula (2) or (3).

[0038] [ka]

[0039] [ka]

[0040] In the formula (2), R 1 R represents a hydrogen atom or an organic group. 2 represents a direct bond or a divalent organic group. 3 ,R 4 Each independently represents a hydrogen atom or an organic group. Z represents a divalent organic group. R 1 ~R 4The organic groups of Z may have a substituent. In the formulas (2) to (3), * indicates a bonding site. The bonding site is a site that bonds to each of the two oxygen atoms bonded to X in the formula (1).

[0041] Formula (2) and formula (3) can be said to be partial structural formulas that represent a partial structure of formula (1). In this specification, the structural units represented by formula (2) and formula (3) may be referred to as structural unit B and structural unit C, respectively. Structural unit B and structural unit C can be said to be partial structures of structural unit A. Also, the structures in which -O- is bonded to the bonding sites in formula (2) and formula (3), respectively, can be regarded as structural units.

[0042] In the formula (2), R 1 R represents a hydrogen atom or an organic group. In this specification, an organic group is a functional group having at least one carbon atom. 1 The organic group may have a substituent.

[0043] The number of carbon atoms in the organic group is not particularly limited, but is preferably 1 to 30. The number of carbon atoms is more preferably 1 to 20, and further preferably 1 to 16. When the number of carbon atoms in the organic group is within the above range, the glass transition temperature is high, and the heat resistance is excellent.

[0044] R 1 The organic group is not particularly limited, but specific examples thereof include a hydrocarbon group having 1 to 16 carbon atoms, an acyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 3 to 14 carbon atoms, an acyloxy group having 1 to 10 carbon atoms, a silyl group, a sulfinyl group, a sulfo group, an alkylthio group, an arylthio group, an amino group, a nitro group, a cyano group, a thienyl group, a pyridyl group, and a furyl group.

[0045] Specific examples of the hydrocarbon group having 1 to 16 carbon atoms include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, an aryl group having 3 to 14 carbon atoms, and an aralkyl group having 4 to 16 carbon atoms.

[0046] Examples of the alkyl group having 1 to 12 carbon atoms include chain alkyl groups such as methyl group, ethyl group, propyl group, butyl group, pentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, and dodecyl group, and cycloalkyl groups such as cyclopentyl group and cyclohexyl group. Examples of the alkenyl group having 2 to 10 carbon atoms include chain alkenyl groups such as vinyl group, allyl group, butenyl group, and hexenyl group, and cyclic alkenyl groups such as cyclopentenyl group and cyclohexenyl group. Examples of the alkynyl group having 2 to 10 carbon atoms include ethynyl group, methylethynyl group, 1-propionyl group, acetylene group, and propynyl group. Examples of the aryl group having 3 to 14 carbon atoms include phenyl group, tolyl group, and naphthyl group. Examples of the aralkyl group having 4 to 16 carbon atoms include phenylmethyl group and phenylethyl group.

[0047] Examples of the acyl group having 1 to 10 carbon atoms include an acetyl group and a benzoyl group. Examples of the alkoxy group having 1 to 10 carbon atoms include a methoxy group, an ethoxy group, and a propoxy group. Examples of the aryloxy group having 3 to 14 carbon atoms include a phenoxy group. Examples of the acyloxy group having 1 to 10 carbon atoms include a methoxyacetyl group and a phenoxyacetyl group. Examples of the silyl group include a trimethylsilyl group. Examples of the organic sulfo group include an alkylsulfo group such as a methylsulfonyl group and an ethylsulfonyl group. Examples of the sulfinyl group include a methylsulfinyl group and an ethylsulfinyl group. Examples of the alkylthio group include a methylthio group and an ethylthio group. Examples of the arylthio group include a phenylthio group. Examples of the organic amino group include a dimethylamino group.

[0048] Of these, from the viewpoint of the stability of the polymer itself, R 1is preferably a hydrogen atom or a hydrocarbon group having 1 to 16 carbon atoms which may have a substituent, and from the same viewpoint, is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, an aryl group having 1 to 14 carbon atoms, or an aralkyl group having 4 to 16 carbon atoms. From the viewpoint of the balance between the optical properties, weather resistance, heat resistance, and mechanical properties of the polymer, a hydrogen atom or an alkyl group having 1 to 12 carbon atoms is more preferable, a hydrogen atom or an alkyl group having 1 to 6 carbon atoms is particularly preferable, and a hydrogen atom or an alkyl group having 1 to 3 carbon atoms is most preferable. Specific examples include a hydrogen atom and a methyl group.

[0049] These organic groups may have a substituent. There are no particular limitations on the substituent as long as it does not significantly impair the excellent physical properties of the thermoplastic resin. In addition to the organic groups, examples of the substituent include alkoxy groups (e.g., methoxy, ethoxy, isopropoxy, tert-butoxy, etc.), hydroxyl groups, amino groups, carboxyl groups, ester groups, halogen atoms (e.g., fluorine, chlorine, bromine, iodine, etc.), thiol groups, thioether groups, and organic silicon groups. R 1 The organic group may have one or more of these substituents. When the organic group has two or more substituents, the substituents may be the same or different. In this specification, various substituents (specifically, R 1 ~R 4 When the substituent has a further substituent, the number of carbon atoms of each of the substituents (Z, and Z) refers to the total number of carbon atoms including the number of carbon atoms of the further substituent.

[0050] In the formula (2), R 2 R represents a direct bond or a divalent organic group. 2 The divalent organic group may have a substituent.

[0051] R 2 The number of carbon atoms in the divalent organic group is not particularly limited, but is preferably 1 to 30. The number of carbon atoms is more preferably 1 to 20, and further preferably 1 to 16. When the number of carbon atoms in the divalent organic group is within the above range, the glass transition temperature is high, and the heat resistance is excellent.

[0052] R 2 The divalent organic group is not particularly limited, but is preferably a divalent hydrocarbon group having 1 to 16 carbon atoms. In this case, the glass transition temperature is increased, and the heat resistance of the thermoplastic resin is improved. Specific examples of the divalent hydrocarbon group having 1 to 16 carbon atoms include an alkylene group having 1 to 12 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, an alkynylene group having 2 to 10 carbon atoms, an arylene group having 3 to 14 carbon atoms, and an aralkylene group having 4 to 16 carbon atoms.

[0053] From the viewpoint of increasing the glass transition temperature and improving heat resistance, R 2 is particularly preferably a direct bond or an alkylene group having 1 to 12 carbon atoms.

[0054] R 2 The divalent organic group may have a substituent. The substituent is as defined above for R 1 The same applies to the organic groups of the formula (I).

[0055] Specific examples of the structural unit B are shown in the following [Group I].

[0056] [ka] TIFF0007552158000020.tif120170TIFF0007552158000021.tif113170

[0057] Preferred structural units B are shown in the following group [II]. When the structural unit B is at least one selected from group [II], the balance of heat resistance, mechanical properties, low water absorbency, and moist heat resistance is excellent. [ka]

[0058] More preferred structural units B are shown in the following group [III]. When the structural unit B is at least one selected from group [III], a resin having a good balance of heat resistance, mechanical properties, low water absorbency, and moist heat resistance at a higher level can be obtained. [ka]

[0059] Next, in the formula (3), R 3 , R 4 R each independently represents a hydrogen atom or an organic group. 3 ,R 4 The organic group of R may have a substituent. 3 , R 4 The details of the organic group are as follows: 1 The same is true for

[0060] From the viewpoint of the stability of the polymer itself, R 3 , R 4 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 16 carbon atoms which may have a substituent, and more preferably a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. 3 , R 4 are each more preferably independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, an aryl group having 1 to 14 carbon atoms, or an aralkyl group having 4 to 16 carbon atoms. From the viewpoint of the balance between the optical properties, weather resistance, heat resistance, and mechanical properties of the polymer, R 3 , R 4 are each independently more preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, even more preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and particularly preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Specific examples include a hydrogen atom and a methyl group.

[0061] In the formula (3), Z represents a divalent organic group. The divalent organic group of Z may have a substituent. Z is preferably a divalent hydrocarbon group. In this case, synthesis is relatively easy and a resin having excellent heat resistance can be obtained.

[0062] The carbon number of the divalent organic group of Z is not particularly limited, but is preferably 1 to 30. The carbon number is more preferably 1 to 20, further preferably 1 to 16, and even more preferably 1 to 6. When the carbon number of the divalent organic group is within the above range, the glass transition temperature is high and heat resistance is excellent.

[0063] The divalent organic group of Z is not particularly limited, but is preferably a divalent hydrocarbon group having 1 to 16 carbon atoms, and more preferably a divalent hydrocarbon group having 1 to 6 carbon atoms. In this case, the glass transition temperature is high, and heat resistance is excellent. Specific examples of the divalent hydrocarbon group having 1 to 16 carbon atoms include an alkylene group having 1 to 12 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, an alkynylene group having 2 to 10 carbon atoms, an arylene group having 3 to 14 carbon atoms, and an aralkylene group having 4 to 16 carbon atoms.

[0064] From the viewpoint of the stability of the polymer itself, Z is preferably an alkylene group having 1 to 12 carbon atoms, an arylene group having 1 to 14 carbon atoms, or an aralkylene group having 4 to 16 carbon atoms. From the viewpoint of the balance between the optical properties, weather resistance, heat resistance, and mechanical properties of the polymer, Z is more preferably an alkylene group having 1 to 12 carbon atoms, further preferably an alkylene group having 1 to 6 carbon atoms, and particularly preferably an alkylene group having 1 to 3 carbon atoms, such as a methylene group, an ethylene group, or an n-propylene group.

[0065] Specific examples of the structural unit C are shown in the following [Group IV].

[0066] [ka] TIFF0007552158000025.tif86170

[0067] A preferable structural unit C is shown in the following [V]. When the structural unit C is at least one selected from the group [V], a resin having a good balance of heat resistance, mechanical properties, low water absorbency, and moist heat resistance at a higher level can be obtained. [ka]

[0068] The carbonate-based resin may have only the structural unit B, may have only the structural unit C, or may have both the structural unit B and the structural unit C. In addition, in the structural unit B and the structural unit C of the carbonate-based resin, R 1 ~R 4 may be the same or different. The structural units B and C are structural units that are mainly responsible for the excellent heat resistance of carbonate-based resins by introducing their rigid molecular structures into the polymer chain.

[0069] From the viewpoint of the heat resistance and optical properties of the resin, it is preferable that the carbonate-based resin contains the structural unit C represented by the formula (3). That is, it is preferable that the carbonate-based resin contains the structural unit A represented by the formula (1), and X in the formula (1) is a structure represented by the formula (3). In particular, in the formula (3), R 3 and R 4 It is particularly preferable that is an optionally substituted alkyl group having 1 to 12 carbon atoms, and Z is an optionally substituted divalent alkylene group having 1 to 12 carbon atoms.

[0070] It is particularly preferable that the carbonate-based resin has a structural unit represented by the following formula (4) or a structural unit represented by the following formula (5). That is, it is preferable that formula (3) is formula (4) or formula (5). In this case, the obtained resin has excellent and well-balanced optical properties, heat resistance, and melt processability. [ka] [ka] In the formulas (4) and (5), * indicates a binding site.

[0071] In the carbonate-based resin, there is no particular limitation on the weight ratio of the structural unit A described above, but from the viewpoint of extremely excellent heat resistance of the resin, it is preferable that the resin is a homopolycarbonate resin in which all structural units constituting the resin are structural units A. In this case, as described later, it is predicted from the Flory-Fox equation that a resin having a high glass transition temperature and extremely excellent heat resistance can be obtained.

[0072] From the viewpoint of achieving an excellent balance between heat resistance and mechanical properties of the resin, when the total weight of all structural units and linking groups constituting the resin is taken as 100% by weight, the content of the structural unit A represented by the formula (1) is preferably 1% by weight or more and 99% by weight or less. This ratio is more preferably 10% by weight or more, even more preferably 20% by weight or more, and particularly preferably 30% by weight or more. This ratio is more preferably 85% by weight or less, even more preferably 80% by weight or less, and particularly preferably 75% by weight or less. When the content of the structural unit A is within the above range, the resin has an excellent balance between heat resistance and mechanical properties.

[0073] On the other hand, when focusing on the content of structural unit B and structural unit C in the carbonate-based resin, from the viewpoint of excellent balance between heat resistance and mechanical properties of the resin, when the total weight of all structural units and linking groups constituting the resin is taken as 100% by weight, the total content of structural unit B and structural unit C is preferably 1% by weight or more and 95% by weight or less. This ratio is more preferably 10% by weight or more, even more preferably 20% by weight or more, and particularly preferably 30% by weight or more. This ratio is more preferably 85% by weight or less, even more preferably 80% by weight or less, and particularly preferably 75% by weight or less. When the total content of structural unit B and structural unit C is within the above range, the resin has an excellent balance between heat resistance and mechanical properties.

[0074] In the carbonate-based resin, the cyclohexane rings in the structural units B and C are preferably inositol residues derived from inositol. Specific examples of the inositol include all-cis-inositol, epi-inositol, allo-inositol, muco-inositol, myo-inositol, neo-inositol, chiro-D-inositol, chiro-L-inositol, and scyllo-inositol. From the viewpoint of easy availability of raw materials, it is preferable that the inositol residues are derived from myo-inositol, that is, the structural units B and C in the carbonate-based resin are introduced using myo-inositol and / or a derivative thereof as a raw material dihydroxy compound in the production method of the polycarbonate resin described below.

[0075] (Structural units other than structural unit A) As described above, the carbonate-based resin may be a homopolycarbonate resin consisting of only the structural unit A, or may be a copolymer having a structural unit other than the structural unit A. The carbonate-based resin is preferably a copolymer containing, in addition to the structural unit A, a structural unit derived from at least one dihydroxy compound selected from the group consisting of an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, a heteroalicyclic dihydroxy compound, and an aromatic dihydroxy compound. Since these dihydroxy compounds have a flexible molecular structure, the mechanical properties (especially the toughness) of the resin are improved by containing a structural unit derived from these compounds, and a resin having a good balance between heat resistance and mechanical properties can be obtained. In addition, it is more preferable that the carbonate-based resin contains at least one of a structural unit derived from an alicyclic dihydroxy compound and a structural unit derived from a heteroalicyclic dihydroxy compound, and a structural unit represented by the formula (1).

[0076] In this specification, the term "alicyclic dihydroxy compound" refers to a carbocyclic dihydroxy compound that does not have aromaticity. In addition, the term "heteroalicyclic dihydroxy compound" refers to a cyclic dihydroxy compound that contains one or more heteroatoms as ring-constituting atoms (excluding dihydroxy compounds represented by formula (11) and formula (12) described below). In this specification, the term "heteroalicyclic dihydroxy compound" refers to a concept that does not include the above-mentioned alicyclic dihydroxy compounds.

[0077] Preferred specific examples of the structural unit derived from at least one dihydroxy compound selected from the group consisting of aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, heteroalicyclic dihydroxy compounds, and aromatic dihydroxy compounds include structural units D1 to D4 and structural units D6 to D7 described later.

[0078] The carbonate-based resin is preferably a copolymer containing, in addition to the structural unit A, a structural unit derived from at least one dicarboxylic acid compound selected from the group consisting of an aliphatic dicarboxylic acid compound, an alicyclic dicarboxylic acid compound, a heteroalicyclic dicarboxylic acid compound, and an aromatic dicarboxylic acid compound. In this case, a resin having a good balance between heat resistance and mechanical properties is obtained. In addition, when the carbonate-based resin is composed of the structural unit A and the structural unit derived from the above-mentioned dicarboxylic acid compound, it becomes a polyester carbonate.

[0079] In this specification, alicyclic dicarboxylic acid compound is defined as a carbocyclic dicarboxylic acid compound that does not have aromaticity.In addition, heteroalicyclic dicarboxylic acid compound is defined as a cyclic dicarboxylic acid compound that contains one or more heteroatoms as ring-constituting atoms.In this specification, heteroalicyclic dicarboxylic acid compound is a concept that does not include the above-mentioned alicyclic dicarboxylic acid compound.

[0080] Preferred specific examples of the structural unit derived from one or more dicarboxylic acid compounds selected from the group consisting of aliphatic dicarboxylic acid compounds, alicyclic dicarboxylic acid compounds, heteroalicyclic dicarboxylic acid compounds, and aromatic dicarboxylic acid compounds include the structural unit D5 described later.

[0081] When the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by weight, it is preferable that the structural unit (excluding the structural unit A) derived from at least one dihydroxy compound selected from the group consisting of aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, and heteroalicyclic dihydroxy compounds is contained in an amount of 1% by weight or more and 95% by weight or less. In this case, a resin having a good balance between high heat resistance and other physical properties is obtained. The content of the structural unit derived from at least one dihydroxy compound selected from the group consisting of aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, and heteroalicyclic dihydroxy compounds is more preferably 15% by weight or more, and even more preferably 20% by weight or more. Also, it is more preferably 90% by weight or less, and even more preferably 80% by weight or less.

[0082] (Structural unit D1) The carbonate-based resin preferably contains a structural unit D1 represented by the following formula (6).

[0083] [ka]

[0084] The weight ratio of the structural unit D1 is preferably 1% by weight or more and 95% by weight or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin (specifically, carbonate-based resin) is taken as 100% by weight. This ratio is more preferably 20% by weight or more, and particularly preferably 30% by weight or more. Also, it is more preferably 80% by weight or less, and particularly preferably 70% by weight or less.

[0085] If the content of the structural unit D1 is more than the above range, the heat resistance becomes excessively high, and the mechanical properties and melt processability deteriorate. In addition, since the structural unit represented by the formula (6) has a highly hygroscopic structure, if the content is too high, the water absorption rate of the resin increases, and there is a concern that the optical properties of the molded product may change or deformation or cracking may occur in a high humidity environment. On the other hand, if the content of the structural unit D1 is less than the above range, the heat resistance becomes insufficient, and the optical properties such as high transmittance and low photoelastic coefficient, which are the characteristics of polycarbonate resin, cannot be obtained.

[0086] Examples of dihydroxy compounds into which the structural unit D1 can be introduced include isosorbide (ISB), isomannide, and isoidet (hereinafter, these may be referred to as "dihydroxy compound D1"), which are stereoisomers. These may be used alone or in combination of two or more. Among these, it is particularly preferable to use ISB from the viewpoints of availability and polymerization reactivity.

[0087] The dihydroxy compound D1 may contain a stabilizer such as a reducing agent, an antioxidant, an oxygen scavenger, a light stabilizer, an antacid, a pH stabilizer, or a heat stabilizer. Since the dihydroxy compound D1 is particularly susceptible to deterioration under acidic conditions, it is preferable to contain a basic stabilizer.

[0088] Examples of the basic stabilizer include hydroxides, carbonates, phosphates, phosphites, hypophosphites, borates, and fatty acid salts of metals in Group 1 or 2 of the long-form periodic table (Nomenclature of Inorganic Chemistry IUPAC Recommendations 2005); tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylphenylammonium hydroxide, triethylmethylammonium hydroxide, triethylbenzylammonium hydroxide, triethylphenylammonium hydroxide, tributylbenzylammonium hydroxide, tributylphenylammonium hydroxide, tetraphenylammonium hydroxide, benzyltriphenylammonium hydroxide, methyltriphenylammonium hydroxide, and bromide. basic ammonium compounds such as ethyltriphenylammonium hydroxide; diethylamine, dibutylamine, triethylamine, morpholine, N-methylmorpholine, pyrrolidine, piperidine, 3-amino-1-propanol, ethylenediamine, N-methyldiethanolamine, diethylethanolamine, diethanolamine, triethanolamine, 4-aminopyridine, 2-aminopyridine, N,N-dimethyl-4-aminopyridine, 4-diethylaminopyridine, 2-hydroxypyridine, 2-methoxypyridine, 4-methoxypyridine, 2-dimethylaminoimidazole, 2-methoxyimidazole, imidazole, 2-mercaptoimidazole, 2-methylimidazole, aminoquinoline, and the like; amine compounds, and hindered amine compounds such as di-(tert-butyl)amine and 2,2,6,6-tetramethylpiperidine.

[0089] There is no particular restriction on the content of these basic stabilizers in dihydroxy compound D1. However, since dihydroxy compound D1 is unstable under acidic conditions, it is preferable to add the stabilizers so that the pH of an aqueous solution of dihydroxy compound D1 containing the stabilizers is around 7.

[0090] If the amount of stabilizer is too small, the effect of preventing deterioration of dihydroxy compound D1 may not be obtained, whereas if the amount is too large, it may lead to denaturation of dihydroxy compound D1. Therefore, the amount of stabilizer is preferably 0.0001% by weight to 0.1% by weight, and more preferably 0.001% by weight to 0.05% by weight, relative to dihydroxy compound D1.

[0091] In addition, since dihydroxy compound D1 easily absorbs moisture and gradually deteriorates due to oxygen, it is preferable to prevent moisture from mixing with the compound during storage or handling during production, and to use an oxygen scavenger or to store the compound under a nitrogen atmosphere.

[0092] (Structural unit D2) The carbonate-based resin preferably contains a structural unit D2 represented by the following formula (7).

[0093] [ka]

[0094] The weight ratio of the structural unit D2 is preferably 1% by weight or more and 95% by weight or less, when the total weight of all structural units and linking groups constituting the carbonate-based resin is taken as 100% by weight. This ratio is more preferably 20% by weight or more, and particularly preferably 30% by weight or more. Moreover, it is more preferably 80% by weight or less, and particularly preferably 70% by weight or less.

[0095] If the content of the structural unit D2 is more than the above range, the heat resistance becomes excessively high, and the mechanical properties and melt processability deteriorate. In addition, since the structural unit represented by the formula (7) has a highly hygroscopic structure, if the content is too high, the water absorption rate of the resin increases, and there is a concern that the optical properties of the molded product may change, or deformation or cracking may occur in a high-humidity environment. On the other hand, if the content of the structural unit D2 is less than the above range, the heat resistance becomes insufficient, and the optical properties such as high transmittance and low photoelastic coefficient, which are the characteristics of polycarbonate resin, cannot be obtained.

[0096] Examples of dihydroxy compounds that can introduce the structural unit D2 include 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane (common name: spiro glycol), 3,9-bis(1,1-diethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, 3,9-bis(1,1-dipropyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, and dioxane glycol. Among these, spiro glycol is particularly preferred from the viewpoints of easy availability and high glass transition temperature of the resin. These may be used alone or in combination of two or more.

[0097] (fluorene structural unit) The carbonate-based resin may contain a structural unit selected from structural units represented by the following formulas (8) to (10). The structural units represented by the following formulas (8) to (10) may be referred to as structural unit D3, structural unit D4, and structural unit D5, respectively. The structural units represented by the following formulas (8) to (10) may be collectively referred to as "fluorene-based structural units", and a bifunctional monomer containing a fluorene-based structural unit may be referred to as a "fluorene-based monomer". The structural units represented by the following formulas (9) and (10) may be referred to as "oligofluorene structural units".

[0098] [ka]

[0099] In the formula (8), R 5 ~R 8each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 6 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, and X represents a substituted or unsubstituted alkylene group having 2 to 10 carbon atoms, a substituted or unsubstituted cycloalkylene group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms. m and n each independently represent an integer of 0 to 5.

[0100] [ka] [ka]

[0101] (In formulas (9) and (10), R 9 ~R 11 each independently represents a direct bond or an alkylene group having 1 to 4 carbon atoms which may have a substituent, R 12 ~R 17 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an aryl group having 4 to 10 carbon atoms which may have a substituent, an acyl group having 1 to 10 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an aryloxy group having 1 to 10 carbon atoms which may have a substituent, an acyloxy group having 1 to 10 carbon atoms which may have a substituent, an amino group which may have a substituent, a vinyl group having 1 to 10 carbon atoms which may have a substituent, an ethynyl group having 1 to 10 carbon atoms which may have a substituent, a sulfur atom which has a substituent, a silicon atom which has a substituent, a halogen atom, a nitro group, or a cyano group, provided that R 12 ~R 17 At least two adjacent groups among these may be bonded to each other to form a ring.)

[0102] By introducing the fluorene-based structural unit, it becomes possible to adjust the wavelength dispersion (wavelength dependency) of the retardation. Many polymers have a positive wavelength dispersion in which the retardation becomes larger as the wavelength becomes shorter, but the fluorene-based structural unit has a reverse wavelength dispersion in which the retardation becomes smaller as the wavelength becomes shorter, so that it is possible to adjust the wavelength dispersion from flat to reverse depending on the content of the fluorene-based structural unit.

[0103] The expression of reverse wavelength dispersion by the fluorene-based structural units represented by the formulas (8) to (10) varies depending on the structure. In order to obtain optimal wavelength dispersion characteristics as a retardation film, the content of the fluorene-based structural units is preferably 1% by weight or more and 70% by weight or less, more preferably 5% by weight or more and 60% by weight or less, and particularly preferably 10% by weight or more and 50% by weight or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by weight.

[0104] If the content of the fluorene-based structural unit in the resin is too small, the effect of containing these structural units cannot be obtained sufficiently, but since the fluorene-based structural unit has negative birefringence, if the content in the resin is more than the above range, the birefringence becomes too small, and desired retardation cannot be obtained.In addition, the ratio of other copolymerization components becomes small, and it may become difficult to adjust the balance of other properties such as heat resistance and mechanical properties.

[0105] Specific examples of the dihydroxy compound used to introduce the structural unit D3 represented by the formula (8) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4- (2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene, and the like.

[0106] Among the above dihydroxy compounds, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene are particularly preferred from the viewpoints of excellent properties such as heat resistance, optical properties, and mechanical properties, and of easy availability.

[0107] R in the formula (9) and the formula (10) 9 and R 10 In the above, examples of the "alkylene group having 1 to 4 carbon atoms which may have a substituent" include the following alkylene groups. Linear alkylene groups such as methylene, ethylene, n-propylene, and n-butylene; and branched alkylene groups such as methylmethylene, dimethylmethylene, ethylmethylene, propylmethylene, (1-methylethyl)methylene, 1-methylethylene, 2-methylethylene, 1-ethylethylene, 2-ethylethylene, 1-methylpropylene, 2-methylpropylene, 1,1-dimethylethylene, 2,2-dimethylpropylene, and 3-methylpropylene. 9 and R 10 The positions of the branched chains in the formula are indicated by numbers given so that the carbon atom on the fluorene ring side is at the 1st position.

[0108] R 9 and R 10 The selection of R has a particularly important effect on the development of reverse wavelength dispersion. The strongest reverse wavelength dispersion is exhibited when the fluorene ring in the fluorene monomer structure is oriented perpendicular to the main chain direction (stretching direction). In order to bring the orientation state of the fluorene ring closer to the above state and develop strong reverse wavelength dispersion, it is necessary to select R having an alkylene group with 2 to 3 carbon atoms on the main chain. 9 and R 10 is preferably adopted. When the carbon number is 1, unexpectedly, reverse wavelength dispersion may not be exhibited. This may be due to the steric hindrance of the carbonate group or ester group, which is the linking group of the oligofluorene structural unit, causing the orientation of the fluorene ring to be fixed in a direction that is not perpendicular to the main chain direction. On the other hand, when the carbon number is too large, the fixation of the orientation of the fluorene ring may be weakened, which may weaken the reverse wavelength dispersion. In addition, the heat resistance of the resin also tends to decrease.

[0109] As shown in the formulas (7) and (8), R 9 and R 10has one end of an alkylene group bonded to a fluorene ring, and the other end bonded to either an oxygen atom or a carbonyl carbon contained in a linking group. From the viewpoints of thermal stability, heat resistance, and reverse wavelength dispersion, it is preferable that the other end of the alkylene group is bonded to a carbonyl carbon. As will be described later, specific examples of monomers having an oligofluorene structure include diol or diester (hereinafter, diester also includes dicarboxylic acid) structures, and it is preferable to use a diester as a raw material for polymerization. From the viewpoint of facilitating production, R 9 and R 10 It is preferable to employ the same alkylene group for each of the groups.

[0110] R 11 In the above, examples of the "alkylene group having 1 to 4 carbon atoms which may have a substituent" include the following alkylene groups. Straight-chain alkylene groups such as a methylene group, an ethylene group, an n-propylene group, or an n-butylene group; and branched-chain alkylene groups such as a methylmethylene group, a dimethylmethylene group, an ethylmethylene group, a propylmethylene group, a (1-methylethyl)methylene group, a 1-methylethylene group, a 2-methylethylene group, a 1-ethylethylene group, a 2-ethylethylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,1-dimethylethylene group, a 2,2-dimethylpropylene group, or a 3-methylpropylene group.

[0111] R 11 The alkylene group preferably has 1 to 2 carbon atoms on the main chain, and more preferably has 1 carbon atom. 11 If you adopt R 9 and R 10 Similarly, the fixation of the fluorene rings is weakened, which may lead to a decrease in reverse wavelength dispersion, an increase in the photoelastic coefficient, a decrease in heat resistance, etc. On the other hand, the fewer the number of carbon atoms on the main chain, the better the optical properties and heat resistance, but when the 9-positions of two fluorene rings are directly bonded, the thermal stability is deteriorated.

[0112] The fluorene ring contained in the oligofluorene structural unit is R12 ~R 17 are all hydrogen atoms, or R 12 and / or R 17 is any one selected from the group consisting of a halogen atom, an acyl group, a nitro group, a cyano group, and a sulfo group, and R 13 ~R 16 is preferably a hydrogen atom. In the former case, the compound containing the oligofluorene structural unit can be derived from fluorene, which is industrially inexpensive. In the latter case, the reactivity of the 9-position of the fluorene ring is improved, so that various derivatization reactions tend to be applicable in the synthesis process of the compound containing the oligofluorene structural unit. The fluorene ring is more preferably, 12 ~R 17 are all hydrogen atoms, or R 12 and / or R 17 is any one selected from the group consisting of a fluorine atom, a chlorine atom, a bromine atom, and a nitro group, and R 13 ~R 16 is a hydrogen atom, 12 ~R 17 It is particularly preferable that all of are hydrogen atoms. By adopting the above-mentioned configuration, the fluorene ratio can be increased, and steric hindrance between the fluorene rings is unlikely to occur, and desired optical properties derived from the fluorene rings tend to be obtained.

[0113] Among the divalent oligofluorene structural units represented by the formulas (7) and (8), preferred structures include structures having skeletons represented by the formulas (A1) to (A6), specifically exemplified in the following group [A].

[0114] [ka]

[0115] Examples of the monomer having an oligofluorene structural unit include a specific dihydroxy compound represented by the following formula (7A) and a specific diester represented by the following formula (8A).

[0116] [ka]

[0117] In the formulas (7A) and (8A), R 9 ~R 17 are the same as in the above formulas (7) and (8). 1 and A 2 is a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, A 1 and A 2 may be the same or different.

[0118] As the monomer having the divalent oligofluorene structural unit, it is preferable to use the specific diester represented by the formula (8A). The specific diester has relatively better thermal stability than the specific dihydroxy compound represented by the formula (7A), and the fluorene ring in the polymer tends to be oriented in a preferred direction, and to show stronger reverse wavelength dispersion. In addition, when the polycarbonate resin contains the structural unit of the diester, this resin is called a polyester carbonate resin.

[0119] A in the above formula (8A) 1 and A 2 When A in the formula (8A) is a hydrogen atom or an aliphatic hydrocarbon group such as a methyl group or an ethyl group, the polymerization reaction may not occur easily under the polymerization conditions of a polycarbonate that are usually used. 1 and A 2 is preferably an aromatic hydrocarbon group.

[0120] ·Structural unit D6 / Structural unit D7 From the viewpoint of imparting toughness to the resin and improving mechanical properties, the carbonate-based resin may further have a structural unit D6 derived from an aliphatic dihydroxy compound and / or a structural unit D7 derived from an alicyclic dihydroxy compound. The structural units D6 and D7 are not intended to include not only the structural unit A and the structural units D1 to D5, but also the structural unit D8 described below. Examples of the aliphatic dihydroxy compound include linear aliphatic dihydroxy compounds and branched aliphatic dihydroxy compounds, but do not include alicyclic dihydroxy compounds.

[0121] Examples of linear aliphatic dihydroxy compounds include ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-pentanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, polypropylene glycol, polytrimethylene glycol, polytetramethylene glycol, and polydecamethylene glycol.

[0122] Examples of the branched aliphatic hydrocarbon dihydroxy compound include neopentyl glycol and hexylene glycol.

[0123] From the viewpoint of imparting flexibility to the carbonate-based resin and improving the toughness of the resin, the dihydroxy compound constituting the structural unit D6 is particularly preferably a linear aliphatic dihydroxy compound having a primary hydroxyl group. Examples of linear aliphatic dihydroxy compounds having a primary hydroxyl group include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,10-decanediol, and 1,12-dodecanediol.

[0124] From the viewpoint of further improving mechanical properties such as toughness, the content of the structural unit D6 in the carbonate-based resin is preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 25% by mass or more, and particularly preferably 30% by mass or more, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by mass. Also, it is preferably 95% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, and particularly preferably 50% by mass or less. From the viewpoint of achieving both heat resistance and mechanical strength, the content of the structural unit D6 in the carbonate-based resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, even more preferably 4% by mass or more, particularly preferably 5% by mass or more, preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by mass.

[0125] Examples of the alicyclic dihydroxy compound include 1,2-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and dihydroxy compounds derived from terpene compounds such as limonene.

[0126] From the viewpoint of imparting flexibility to the carbonate-based resin and improving the toughness of the resin, the dihydroxy compound constituting the structural unit D7 is preferably 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, or the like.

[0127] From the viewpoint of achieving both heat resistance and mechanical strength, the content of the structural unit D7 in the carbonate-based resin is preferably 1 mass% or more, more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, and particularly preferably 40 mass% or more, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 mass%, and is preferably 95 mass% or less, more preferably 90 mass% or less, even more preferably 80 mass% or less, even more preferably 70 mass% or less, and particularly preferably 60 mass% or less.

[0128] (Structural unit D8) The polycarbonate resin may contain a structural unit other than the structural units D1 to D7 described above (hereinafter, may be referred to as "structural unit D8"). Examples of monomers containing the structural unit D8 include dihydroxy compounds containing an acetal ring, oxyalkylene glycols, dihydroxy compounds containing an aromatic component, diester compounds, and the like.

[0129] As the dihydroxy compound containing an acetal ring, for example, dioxane glycol represented by the following structural formula (15) can be used.

[0130] [ka]

[0131] As the oxyalkylene glycol, for example, the following dihydroxy compounds can be used. Diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol.

[0132] As the dihydroxy compound containing an aromatic component, for example, the following dihydroxy compounds can be used. 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl )methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(4-hydroxyphenyl)pentane, Bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4, Aromatic bisphenol compounds such as 4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group, such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone.

[0133] As the diester compound, for example, the following dicarboxylic acids can be used. Aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and decalin-2,6-dicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. These dicarboxylic acid components can be used as raw materials for polyester carbonate as dicarboxylic acids themselves, but depending on the production method, dicarboxylic acid esters such as methyl esters and phenyl esters, and dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials.

[0134] From the viewpoint of optical properties, it is preferable to use the other structural units listed above that do not contain aromatic components, but in order to balance heat resistance, mechanical properties, etc. while ensuring optical properties, it may be effective to incorporate aromatic components into the main chain or side chain of the polymer. In this case, for example, aromatic components can be introduced into the polymer by the other structural units containing aromatic structures, but the content of these structural units in the polycarbonate resin, i.e., aromatic structural units other than the structural units represented by the formulas (6) to (8), is preferably 5% by weight or less when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by weight. If the amount of other structural units containing aromatic structures increases, there is a concern that the photoelastic coefficient will deteriorate.

[0135] Since the polymerization reactivity of diester compounds is relatively low, from the viewpoint of increasing the reaction efficiency, it is more preferable not to use diester compounds other than diester compounds having an oligofluorene structural unit.

[0136] The dihydroxy compound or diester compound for introducing the structural unit D8 may be used alone or in combination of two or more depending on the required performance of the resulting resin. The content of the other structural units in the resin is preferably 1% by weight or more and 95% by weight or less, more preferably 10% by weight or more, and particularly preferably 20% by weight or more, when the total weight of all structural units constituting the polycarbonate resin and the weight of the linking group is taken as 100% by weight. Also, it is more preferably 80% by weight or less, and particularly preferably 70% by weight or less. The other structural units mainly play a role in adjusting the heat resistance of the resin and imparting flexibility and toughness, so if the content is too low, the mechanical properties and melt processability of the resin may deteriorate, and if the content is too high, the heat resistance and optical properties may deteriorate.

[0137] (carbonic acid diester) The linking group of the structural unit contained in the polycarbonate resin is introduced by polymerizing a carbonate diester represented by the following formula (16).

[0138] [ka]

[0139] (In formula (11), A 3 and A 4 each represents an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, 3 and A 4 may be the same or different.)

[0140] A 3 and A 4 is preferably a substituted or unsubstituted aromatic hydrocarbon group, more preferably an unsubstituted aromatic hydrocarbon group. Examples of the substituent of the aliphatic hydrocarbon group include an ester group, an ether group, an amide group, and a halogen atom, and examples of the substituent of the aromatic hydrocarbon group include an alkyl group such as a methyl group or an ethyl group.

[0141] Examples of the carbonic acid diester represented by the formula (16) include diphenyl carbonate (hereinafter sometimes abbreviated as DPC), substituted diphenyl carbonate such as ditolyl carbonate, and dialkyl carbonate such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate, with diphenyl carbonate and substituted diphenyl carbonate being preferred, and diphenyl carbonate being particularly preferred.

[0142] The carbonate diester may contain impurities such as chloride ions, and these impurities may inhibit the polymerization reaction or deteriorate the hue of the resulting resin. Therefore, it is preferable to use a diester that has been purified, as necessary, by distillation or the like.

[0143] In addition, when a polymerization reaction is carried out using both the diester monomer represented by the formula (8A) and the carbonate diester represented by the formula (16), 1 , A 2 and A in the formula (16) 3 , A 4 If all of the A have the same structure, the components released during the polymerization reaction are the same, making it easier to recover and reuse the components. 1 ~A 4 is particularly preferably a phenyl group. 1 ~A 4 When is a phenyl group, the component which is eliminated during the polymerization reaction is phenol.

[0144] From the viewpoint of excellent heat resistance of the resin, the carbonate-based resin is preferably a copolymer having the structural unit A and at least one structural unit selected from the group consisting of the structural unit D1, the structural unit D2, the structural unit D3, the structural unit D4, the structural unit D5, the structural unit D6, and the structural unit D7. From the viewpoint of obtaining better heat resistance, the carbonate-based resin is more preferably a copolymer having the structural unit A and at least one structural unit selected from the group consisting of the structural unit D1, the structural unit D2, the structural unit D5, and the structural unit D7, and from the same viewpoint, it is more preferable to have the structural unit A and at least one of the structural unit D1 and the structural unit D2. It is particularly preferable that the carbonate-based resin has the structural unit A, the structural unit D1, and the structural unit D7. In this case, a resin having a good balance of heat resistance, optical properties, and mechanical properties at a high level is obtained.

[0145] [Dihydroxy compound A] The structural units B and C in the carbonate-based resin can be introduced into the carbonate-based resin by using dihydroxy compounds represented by the following formulas (11) and (12), respectively (hereinafter, these may be referred to as "dihydroxy compound A") as raw material dihydroxy compounds in the production method of the carbonate-based resin described below.

[0146] [ka]

[0147] [ka]

[0148] In the formulas (11) to (12), R 1 ~R 4 and Z have the same meanings as in the above formulas (2) to (3), respectively.

[0149] Specific examples of the dihydroxy compound represented by the formula (11) are shown in the following group [VI].

[0150] [ka] TIFF0007552158000041.tif226170

[0151] Among the group [VI], preferred dihydroxy compounds are shown in the following group [VII]. [ka]

[0152] Among the group [VII], more preferred dihydroxy compounds are shown in the following group [VIII]. [ka]

[0153] Specific examples of the dihydroxy compound represented by formula (12) are shown in the following group [IX].

[0154] [ka] TIFF0007552158000045.tif81170

[0155] Among the group [IX], preferred dihydroxy compounds are shown in the following group [X]. [ka]

[0156] Among the dihydroxy compounds A, the dihydroxy compound represented by formula (12) is preferred from the viewpoint of the balance between heat resistance and mechanical properties. 3 and R 4It is particularly preferred that R is an optionally substituted alkyl group having 1 to 12 carbon atoms and Z is an optionally substituted divalent alkylene group having 1 to 12 carbon atoms. In this case, the carbonate resin obtained by polymerizing this has excellent heat resistance.

[0157] Among the dihydroxy compounds represented by the formula (12), those represented by the following formula (13) or formula (14) are particularly preferred. In this case, the carbonate-based resin obtained by polymerizing this compound has excellent heat resistance and mechanical properties in a well-balanced manner.

[0158] [ka]

[0159] [ka]

[0160] The method for producing the dihydroxy compounds represented by the formulas (13) and (14) is not particularly limited, but they can be produced, for example, by the following method.

[0161] [ka]

[0162] Compound 3 is used as a raw material and is converted into compound 4 or compound 7 by a condensation reaction with tetramethoxypropane or tetramethoxypentane in the presence of an acid catalyst. The ester moiety is then hydrolyzed in the presence of a base catalyst to give the dihydroxy compound represented by formula 13 or formula 14.

[0163] The method for producing the raw material compound 3 is not particularly limited, but for example, a method is known in which myo-inositol (1) is reacted with trimethyl orthoacetate in the presence of an acid catalyst. Specifically, the method disclosed in JP 2017-110204 A is known.

[0164] [Method of producing carbonate-based resin] The polycarbonate resin can be produced by a commonly used polymerization method. For example, it can be produced by a solution polymerization method or an interfacial polymerization method using phosgene or a carboxylic acid halide, or a melt polymerization method in which a reaction is carried out without using a solvent. Among these production methods, it is preferable to produce the polycarbonate resin by the melt polymerization method, which is excellent in productivity and can reduce the environmental load because it does not use a solvent or a highly toxic compound.

[0165] In addition, when a solvent is used in polymerization, the solvent may remain in the resin, and the glass transition temperature of the resin may decrease due to the plasticizing effect, which may cause quality fluctuations in processing steps such as molding and stretching, which will be described later. In addition, halogen-based organic solvents such as methylene chloride are often used as solvents, but if the halogen-based solvent remains in the resin, it may cause corrosion of metal parts when a molded product using this resin is incorporated into an electronic device, etc. The resin obtained by the melt polymerization method does not contain a solvent, which is also advantageous for stabilizing processing steps and product quality.

[0166] When producing polycarbonate resin by melt polymerization, a monomer having the structural units described above, a carbonic acid diester, and a polymerization catalyst are mixed and subjected to an ester exchange reaction (also called a polycondensation reaction) under molten conditions, and the reaction rate is increased while removing the elimination components from the system. At the end of the polymerization, the reaction is allowed to proceed under high temperature and high vacuum conditions until the desired molecular weight is reached. When the reaction is complete, the molten resin is removed from the reactor, and the polycarbonate resin is obtained.

[0167] In the polycondensation reaction, the molar ratio of the total dihydroxy compounds and the total diester compounds used in the reaction can be strictly adjusted to control the reaction rate and the molecular weight of the resulting resin. In the case of a polycarbonate resin, the molar ratio of the carbonic acid diester to the total dihydroxy compounds is preferably adjusted to 0.90 to 1.10, more preferably adjusted to 0.96 to 1.05, and particularly preferably adjusted to 0.98 to 1.03. In the case of a polyester carbonate resin, the molar ratio of the total amount of the carbonic acid diester and the total diester compounds to the total dihydroxy compounds is preferably adjusted to 0.90 to 1.10, more preferably adjusted to 0.96 to 1.05, and particularly preferably adjusted to 0.98 to 1.03.

[0168] If the molar ratio is too far above or below the range, it is not possible to produce a resin with the desired molecular weight. If the molar ratio is too small, the number of hydroxyl group terminals in the produced resin increases, which may deteriorate the thermal stability of the resin. Furthermore, a large amount of unreacted dihydroxy compound remains in the resin, which may cause dirt on the molding machine and poor appearance of the molded product in the subsequent molding process. On the other hand, if the molar ratio is too large, the rate of transesterification reaction may decrease under the same conditions, or the amount of remaining carbonic acid diester or diester compound in the produced resin may increase, and these remaining low molecular weight components may also cause problems in the molding process.

[0169] The melt polymerization method is usually carried out in a multi-stage process of two or more stages. The polycondensation reaction may be carried out in two or more stages using one polymerization reactor by sequentially changing the conditions, or may be carried out in two or more stages using two or more reactors by changing the conditions for each stage, but from the viewpoint of production efficiency, it is carried out using two or more, preferably three or more reactors. The polycondensation reaction may be carried out in a batch system, a continuous system, or a combination of a batch system and a continuous system, but from the viewpoint of production efficiency and stability of quality, a continuous system is preferred.

[0170] In polycondensation reactions, it is important to properly control the balance between temperature and pressure in the reaction system. If either the temperature or pressure is changed too quickly, unreacted monomers may be distilled out of the reaction system. As a result, the molar ratio of dihydroxy compounds and diester compounds may change, and a resin with the desired molecular weight may not be obtained.

[0171] In addition, the polymerization rate of the polycondensation reaction is controlled by the balance between the hydroxyl group terminal and the ester group terminal or carbonate group terminal. Therefore, particularly when polymerization is performed in a continuous manner, if the balance of the terminal groups fluctuates due to the distillation of unreacted monomers, it becomes difficult to control the polymerization rate at a constant rate, and the molecular weight of the resulting resin may fluctuate greatly. Since the molecular weight of a resin correlates with the melt viscosity, when the resulting resin is molded, the melt viscosity may fluctuate, leading to problems such as failure to obtain molded products of uniform dimensions.

[0172] Furthermore, when unreacted monomers are distilled off, not only the balance of the terminal groups but also the copolymerization composition of the resin may deviate from the desired composition, which may affect the mechanical properties and optical properties. In the retardation film obtained from the polycarbonate resin, the wavelength dispersion of the retardation is controlled by the ratio of the fluorene monomer and other copolymerization components in the resin, so if the ratio is disturbed during polymerization, the optical properties as designed may not be obtained.

[0173] Below, the melt polycondensation reaction process will be described in two stages: the stage where monomers are consumed to produce oligomers (first-stage reaction), and the stage where polymerization proceeds to the desired molecular weight to produce a polymer (second-stage reaction).

[0174] Specifically, the following conditions can be adopted as reaction conditions in the first stage reaction. That is, the internal temperature of the polymerization reactor is set in the range of usually 130° C. or more, preferably 150° C. or more, more preferably 170° C. or more, and usually 250° C. or less, preferably 240° C. or less, more preferably 230° C. or less. The pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 70 kPa or less, preferably 50 kPa or less, more preferably 30 kPa or less, and usually 1 kPa or more, preferably 3 kPa or more, more preferably 5 kPa or more. The reaction time is set in the range of usually 0.1 hours or more, preferably 0.5 hours or more, and usually 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less.

[0175] The first-stage reaction is carried out while the monohydroxy compound derived from the diester compound generated is distilled out of the reaction system. For example, when diphenyl carbonate is used as the carbonic acid diester, the monohydroxy compound distilled out of the reaction system in the first-stage reaction is phenol.

[0176] In the first stage reaction, the lower the reaction pressure, the more the polymerization reaction can be accelerated, but on the other hand, the more unreacted monomers are distilled off. In order to simultaneously suppress the distillation of unreacted monomers and accelerate the reaction by reducing the pressure, it is effective to use a reactor equipped with a reflux condenser. It is especially good to use a reflux condenser in the early stages of the reaction when there is a lot of unreacted monomers.

[0177] In the second stage reaction, the pressure of the reaction system is gradually lowered from the pressure of the first stage, and the monohydroxy compound generated is removed from the reaction system, and the pressure of the reaction system is finally set to 5 kPa or less, preferably 3 kPa or less, more preferably 1 kPa or less. The internal temperature is usually set to 210°C or more, preferably 220°C or more, and usually 260°C or less, preferably 255°C or less. The reaction time is usually set to 0.1 hours or more, preferably 0.5 hours or more, more preferably 1 hour or more, and usually 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less. In order to suppress side reactions such as coloration, thermal deterioration, and crosslinking and to obtain a resin with good hue and thermal stability, the maximum internal temperature in all reaction stages is preferably 260°C or less, preferably 255°C or less, and more preferably 250°C or less. In particular, if the dihydroxy compound A is subjected to a polymerization reaction at an excessively high temperature, it may decompose to generate branched components, and the resulting polymer may crosslink and gel. If gel is generated, the mechanical properties of the resulting resin may deteriorate, and when used for optical purposes, it will become a foreign matter and deteriorate the appearance quality of the product.

[0178] The transesterification catalyst (hereinafter, sometimes simply referred to as "catalyst" or "polymerization catalyst") that can be used during polymerization can have a very large effect on the reaction rate and the color tone and thermal stability of the resin obtained by polycondensation. The catalyst is not limited as long as it satisfies the transparency, hue, heat resistance, thermal stability, and mechanical strength of the produced resin, and includes basic compounds such as metal compounds of Group 1 or Group 2 (hereinafter, simply referred to as "Group 1" and "Group 2") in the long-form periodic table, basic boron compounds, basic phosphorus compounds, basic ammonium compounds, and amine-based compounds. At least one metal compound selected from the group consisting of metals of Group 2 of the long-form periodic table and lithium is preferably used.

[0179] As the Group 1 metal compound, for example, the following compounds can be used, but it is also possible to use Group 1 metal compounds other than these. Sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium tetraphenylborate, tetraphenylborate potassium tetraphenylborate, lithium tetraphenylborate, cesium tetraphenylborate, sodium benzoate, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, sodium, potassium, lithium and cesium alcoholates and phenolates, and the disodium, dipotassium, dilithium and dicesium salts of bisphenol A. Among these, it is preferable to use lithium compounds from the viewpoints of polymerization activity and the color of the resulting resin.

[0180] As the Group 2 metal compound, for example, the following compounds can be used, but it is also possible to use Group 2 metal compounds other than these. Calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium bicarbonate, barium bicarbonate, magnesium bicarbonate, strontium bicarbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, strontium stearate. Among these, it is preferable to use magnesium compounds, calcium compounds, and barium compounds, and from the viewpoints of polymerization activity and the hue of the obtained resin, it is more preferable to use magnesium compounds and / or calcium compounds, and it is particularly preferable to use calcium compounds.

[0181] It is possible to use, in combination with the Group 1 metal compound and / or Group 2 metal compound, a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound as an auxiliary, but it is particularly preferable to use at least one metal compound selected from the group consisting of metals in Group 2 of the long form periodic table and lithium.

[0182] The amount of the polymerization catalyst used is usually 0.1 μmol to 500 μmol, preferably 0.5 μmol to 300 μmol, more preferably 0.5 μmol to 100 μmol, per 1 mol of the total dihydroxy compounds used in the polymerization, in terms of the metal amount. When at least one metal compound selected from the group consisting of metals of Group 2 of the long periodic table and lithium is used as the polymerization catalyst, particularly when a magnesium compound and / or a calcium compound is used, the polymerization catalyst is usually used in an amount of 0.1 μmol or more, preferably 0.3 μmol or more, and particularly preferably 0.5 μmol or more, per 1 mol of the total dihydroxy compounds, in terms of the metal amount. The amount of the polymerization catalyst used is preferably 300 μmol or less, preferably 100 μmol or less, more preferably 50 μmol or less, and particularly preferably 30 μmol or less, in terms of the metal amount.

[0183] In addition, when a polyester carbonate resin is produced using a diester compound as a monomer, a transesterification catalyst such as a titanium compound, a tin compound, a germanium compound, an antimony compound, a zirconium compound, a lead compound, an osmium compound, a zinc compound, or a manganese compound can be used in combination with or without the basic compound. The amount of these transesterification catalysts used is usually within the range of 1 μmol to 1 mmol, preferably within the range of 5 μmol to 800 μmol, and particularly preferably within the range of 10 μmol to 500 μmol, in terms of the metal amount, relative to 1 mol of the total dihydroxy compounds used in the reaction.

[0184] If the amount of catalyst is too small, the polymerization rate will be slow, and the polymerization temperature will have to be increased accordingly to obtain a resin with a desired molecular weight. This will increase the possibility that the color of the resulting resin will deteriorate, and the unreacted raw materials will volatilize during polymerization, causing the molar ratio of the dihydroxy compound and the diester compound to be disrupted, and the desired molecular weight may not be achieved. On the other hand, if the amount of polymerization catalyst used is too large, undesirable side reactions will occur, which may cause the color of the resulting resin to deteriorate, or the resin to be colored or decomposed during molding.

[0185] Among the group 1 metals, sodium, potassium, and cesium may adversely affect the color if contained in a large amount in the resin. These metals may be mixed not only from the catalyst used, but also from the raw materials and reaction equipment. Regardless of the source, the total amount of compounds of these metals in the resin is preferably 2 μmol or less, preferably 1 μmol or less, and more preferably 0.5 μmol or less per 1 mol of the total dihydroxy compounds.

[0186] After the polycarbonate resin is polymerized as described above, it can usually be cooled and solidified, and pelletized with a rotary cutter, etc. The pelletization method is not limited, but examples thereof include a method in which the polycarbonate resin is withdrawn in a molten state from the final polymerization reactor, cooled and solidified in the form of strands, and pelletized, a method in which the polycarbonate resin is supplied in a molten state from the final polymerization reactor to a single-screw or twin-screw extruder, melt-extruded, cooled and solidified, and pelletized, or a method in which the polycarbonate resin is withdrawn in a molten state from the final polymerization reactor, cooled and solidified in the form of strands, pelletized once, and then supplied to a single-screw or twin-screw extruder again, melt-extruded, cooled and solidified, and pelletized.

[0187] When a diester compound is used in a polycondensation reaction, unreacted diester compounds and by-produced monohydroxy compounds remain in the resin, and they volatilize during melt processing, causing odors that can worsen the working environment, contaminate molding machines, and damage the appearance of molded products. When diphenyl carbonate (DPC), a particularly useful carbonic acid diester, is used, the by-produced phenol has a relatively high boiling point and is not sufficiently removed even by a reaction under reduced pressure, so it tends to remain in the resin.

[0188] The monohydroxy compound derived from the carbonic acid diester contained in the polycarbonate resin is preferably 1000 ppm by weight or less, more preferably 700 ppm by weight or less, and particularly preferably 500 ppm by weight or less. The remaining amount of the carbonic acid diester in the polycarbonate resin is preferably 300 ppm by weight or less, more preferably 200 ppm by weight or less, and particularly preferably 150 ppm by weight or less. In order to solve the above problem, the less the content of the monohydroxy compound and the carbonic acid diester, the better, but it is difficult to reduce the remaining amount in the resin to zero in the melt polymerization method, and excessive effort is required for removal. Usually, the above problem can be sufficiently suppressed by reducing the content of the monohydroxy compound and the carbonic acid diester to 1 ppm by weight, respectively.

[0189] In order to reduce low molecular weight components, including monohydroxy compounds derived from carbonate diesters and carbonate diesters, remaining in the resin, it is effective to subject the resin to a devolatilizing treatment using an extruder and to control the pressure at the end of the polymerization to 3 kPa or less, preferably 2 kPa or less, and more preferably 1 kPa or less.

[0190] When the pressure at the end of the polymerization is reduced, if the reaction pressure is reduced too much, the molecular weight will rise rapidly and the reaction control will become difficult, so it is preferable to produce the resin with an excess of hydroxyl groups or ester groups in the end group concentration, thereby biasing the end group balance. The end group balance can be adjusted by the molar ratio of the total dihydroxy compounds and the total diester compounds charged.

[0191] The specific methods for measuring the content of monohydroxy compounds derived from carbonic acid diesters in polycarbonate resins and the remaining amount of carbonic acid diesters are as described in the Examples section below.

[0192] [Physical properties of carbonate resins] The physical properties of the carbonate-based resin are not particularly limited, but it is preferable that the carbonate-based resin has the following physical properties.

[0193] Reduced Viscosity The molecular weight of carbonate resins can be expressed by reduced viscosity. If the reduced viscosity of the resin is too low, the mechanical strength of the molded product may be reduced. Therefore, the reduced viscosity is usually 0.25 dL / g or more, and preferably 0.30 dL / g or more. On the other hand, if the reduced viscosity of the resin is too high, the fluidity during molding decreases, and the productivity and moldability tend to decrease. Therefore, the reduced viscosity is usually 1.20 dL / g or less, preferably 1.00 dL / g or less, and more preferably 0.80 dL / g or less. The reduced viscosity was measured using a mixed solvent of phenol and 1,1,2,2-tetrachloroethane. The mixture ratio of phenol and 1,1,2,2-tetrachloroethane was 1:1 by mass. The sample concentration was precisely adjusted to 1.00 g / dL, and the measurement was performed using an Ubbelohde viscometer at a temperature of 30.0°C ± 0.1°C.

[0194] Since the reduced viscosity is correlated with the melt viscosity of the resin, the stirring power of the polymerization reactor, the discharge pressure of the gear pump that transports the molten resin, etc. can usually be used as an index for operation management. That is, when the indicated value of the operating device reaches the target value, the polymerization reaction is stopped by returning the pressure of the reactor to normal pressure or by withdrawing the resin from the reactor.

[0195] Glass transition temperature The higher the glass transition temperature of the carbonate-based resin, the more desirable it is when used in applications requiring extremely high heat resistance. On the other hand, when used in applications requiring a balance between high heat resistance, toughness, and melt processability, the glass transition temperature of the carbonate-based resin is preferably 100°C or higher and 200°C or lower. In this case, the glass transition temperature is more preferably 120°C or higher and 180°C or lower, and particularly preferably 130°C or higher and 170°C or lower. The glass transition temperature of the carbonate-based resin is adjusted by the ratio of various structural units constituting the resin. For example, it can be adjusted by the copolymerization ratio of structural units A to C, structural units D1 to D7, and other structural units. If the glass transition temperature is excessively low, the heat resistance tends to deteriorate, and the reliability of various physical properties (optical properties, mechanical properties, dimensions, etc.) of the molded product under the usage environment may deteriorate. On the other hand, if the glass transition temperature is below the above-mentioned upper limit, the heat resistance, toughness, and melt processability are well balanced and excellent.

[0196] ·5% thermogravimetric reduction temperature (Td5) If the 5% thermal weight loss temperature of the carbonate-based resin is high, it is difficult for the resin to thermally decompose. The 5% thermal weight loss temperature of the carbonate-based resin is preferably 300° C. or higher, more preferably 340° C. or higher, and even more preferably 350° C. or higher. The 5% thermal weight loss temperature is specifically measured by the method described in the examples.

[0197] ·Pencil hardness If the hardness of the carbonate-based resin is low, the molded product is easily scratched. The pencil hardness of the carbonate-based resin is preferably B or more, more preferably F or more. From the viewpoint of further improving the scratch resistance of the molded product, the pencil hardness of the carbonate-based resin is more preferably H or more. The pencil hardness is measured by a pencil hardness test. More specifically, the pencil hardness is measured by the method described in the examples. The pencil hardness of the carbonate-based resin is adjusted to the above range by adjusting the type and mixing ratio of the monomers used during production, adjusting the polymerization temperature, or adjusting the amount of additives added.

[0198] Boiling water test The wet heat resistance of a carbonate-based resin can be evaluated based on the presence or absence of deformation caused by a boiling water test. From the viewpoint of excellent wet heat resistance stability, it is preferable that the carbonate-based resin does not deform in the boiling water test.

[0199] Specific methods for measuring the reduced viscosity, glass transition temperature, and 5% thermal weight loss temperature of the carbonate-based resin are as described in the Examples section below.

[0200] Refractive Index Carbonate resins have a refractive index (n D It is preferable that the refractive index (n D ) is more preferably 1.49 to 1.55, and particularly preferably 1.50 to 1.54. The smaller the refractive index, the more the surface reflection of the retardation film can be suppressed, the more the total light transmittance can be improved, and the higher the optical compensation effect. When an aromatic structural unit is contained in a polycarbonate resin in order to impart reverse wavelength dispersion, the refractive index becomes higher compared to a polycarbonate resin composed only of an aliphatic structural unit, but the refractive index can be kept within the above range by minimizing the content of the aromatic structural unit.

[0201] Photoelastic coefficient The photoelastic coefficient of carbonate resin is 30×10 -12 Pa -1 It is preferable that the value is less than 20×10 -12 Pa -1 More preferably, it is 15×10 -12 Pa -1It is particularly preferable that the photoelastic coefficient is 7×10 or less. If the photoelastic coefficient is excessively large, for example, when the carbonate-based resin is used for a retardation film, when the retardation film is laminated with a polarizing plate, the image quality may be deteriorated, such as the periphery of the screen becoming white and blurred. This problem is particularly noticeable when the carbonate-based resin is used in a large display device or a flexible display. When the carbonate-based resin is used for a retardation film, the photoelastic coefficient of the carbonate-based resin is preferably 7×10 or less from the viewpoint of increasing the degree of freedom in controlling other physical properties of the carbonate-based resin. -12 Pa -1 On the other hand, when the carbonate resin is used for an optical film that requires a low retardation, the photoelastic coefficient is preferably 7×10 -12 Pa -1 It is preferable that:

[0202] The carbonate-based resin is composed of, for example, a structural unit represented by any one of the formulas (1) to (3) and an aliphatic structural unit, and does not use other aromatic structural units, so that the photoelastic coefficient can be kept low, as described above.

[0203] ·Saturated water absorption rate If the saturated water absorption rate of the carbonate-based resin is high, the physical properties of the resin change under high humidity, which may reduce the reliability of the molded product. Therefore, the saturated water absorption rate of the carbonate-based resin is preferably 4 wt% or less, more preferably 3.5 wt% or less, even more preferably 3 wt% or less, even more preferably 2.8 wt% or less, and particularly preferably 2.5 wt% or less. The saturated water absorption rate of the carbonate-based resin is measured, for example, by the method described in the Examples. The saturated water absorption rate of the carbonate-based resin is adjusted to the above range by adjusting the type and mixing ratio of the monomers used during production, adjusting the polymerization temperature, and adjusting the amount of additives added.

[0204] The refractive index of polycarbonate resin (n D Specific methods for measuring the elastic modulus, photoelastic coefficient and water absorption are as described in the Examples section below.

[0205] [Resin composition] The polycarbonate resin may contain, within the scope of the object of the present invention, commonly used heat stabilizers, antioxidants, catalyst deactivators, ultraviolet absorbers, light stabilizers, release agents, dyes and pigments, impact modifiers, antistatic agents, slip agents, lubricants, plasticizers, compatibilizers, nucleating agents, flame retardants, inorganic fillers, foaming agents, and the like.

[0206] (Heat stabilizer) If necessary, a heat stabilizer can be blended into the polycarbonate resin in order to prevent a decrease in molecular weight or deterioration in color during melt processing, etc. Examples of such heat stabilizers include commonly known hindered phenol-based heat stabilizers and / or phosphorus-based heat stabilizers.

[0207] As the hindered phenol compound, for example, the following compounds can be used. 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4-methoxyphenol, 2-tert-butyl-4,6-dimethylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-ethylphenol, 2,5-di-tert-butylhydroquinone, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxyphenyl)propionate 2,2'-methylene-bis-(4-methyl-6-tert-butylphenol), 2,2'-methylene-bis-(6-cyclohexyl-4-methylphenol), 2,2'-ethylidene-bis-(2,4-di-tert-butylphenol), tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]-methane, 1,3,5-trimethyl-2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and the like. Among these, it is preferable to use tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]-methane, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, or 1,3,5-trimethyl-2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.

[0208] As the phosphorus-based compound, for example, phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof shown below can be used, but phosphorus-based compounds other than these compounds can also be used. Triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl monoorthoxenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, 4,4'-biphenylenediphosphinic acid tetrakis(2,4-di-tert-butylphenyl), benzenephosphonic acid dimethyl, benzenephosphonic acid diethyl, benzenephosphonic acid dipropyl.

[0209] These heat stabilizers may be used alone or in combination of two or more.

[0210] Such a heat stabilizer may be added to the reaction liquid during melt polymerization, or may be added to the resin using an extruder and kneaded. When forming a film by melt extrusion, the heat stabilizer may be added to the extruder to form a film, or the heat stabilizer may be added in advance to the resin using an extruder and formed into pellets or the like.

[0211] The amount of these heat stabilizers is preferably 0.0001 parts by weight or more, more preferably 0.0005 parts by weight or more, and even more preferably 0.001 parts by weight or more, and is preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, and even more preferably 0.2 parts by weight or less, based on 100 parts by weight of the resin.

[0212] (Polymer alloy) For the purpose of improving mechanical properties, solvent resistance, and other properties, the polycarbonate resin may be kneaded with one or more synthetic resins, such as aromatic polycarbonate, aromatic polyester, aliphatic polyester, polyamide, polystyrene, polyolefin, acrylic, amorphous polyolefin, ABS, AS, polylactic acid, polybutylene succinate, and the like, or rubber, to form a polymer alloy.

[0213] The additives and modifiers can be produced by mixing the components in the resin simultaneously or in any order using a mixer such as a tumbler, V-type blender, Nauter mixer, Banbury mixer, kneading roll, or extruder. Among these, kneading using an extruder, particularly a twin-screw extruder, is preferred from the viewpoint of improving dispersibility.

[0214] [Transparent film and retardation film] The transparent film is formed by molding a thermoplastic resin (specifically, a carbonate-based resin such as a polycarbonate resin). The retardation film is formed by stretching a transparent film in at least one direction. Hereinafter, the transparent film may be referred to as an "unstretched film."

[0215] (Method of manufacturing unstretched film) As a method for forming an unstretched film using a polycarbonate resin, a casting method in which the resin is dissolved in a solvent and cast, and then the solvent is removed, or a melt film-forming method in which the resin is melted without using a solvent to form a film can be adopted.Specific examples of the melt film-forming method include melt extrusion using a T-die, calendar molding, heat pressing, co-extrusion, co-melting, multi-layer extrusion, and inflation molding.The film-forming method for an unstretched film is not particularly limited, but since the casting method may cause problems due to residual solvent, the melt film-forming method is preferable, and among them, the melt extrusion method using a T-die is preferable from the viewpoint of ease of subsequent stretching treatment.

[0216] (Method of manufacturing phase difference film) The unstretched film is stretched and oriented in at least one direction to obtain a retardation film. As the stretching method, a known method such as longitudinal uniaxial stretching, transverse uniaxial stretching using a tenter or the like, or a combination of these, simultaneous biaxial stretching, sequential biaxial stretching, etc. can be used. Stretching may be performed in a batch manner, but continuous stretching is preferable in terms of productivity. Furthermore, compared with the batch manner, continuous stretching can obtain a retardation film with less variation in the in-plane retardation of the film.

[0217] [Application] There are no particular limitations on the uses of the transparent film, but taking advantage of its excellent physical properties such as heat resistance, optical properties, and melt processability, it is suitable for optical films such as retardation films used in various liquid crystal display devices and mobile devices.

[0218] For example, the retardation film obtained by stretching a transparent film is laminated with a known polarizing film and cut to a desired size to form a circular polarizing plate. Such a circular polarizing plate can be used, for example, for compensating the viewing angle of various displays (liquid crystal display devices, organic EL display devices, plasma display devices, FED field emission displays, SED surface field display devices), preventing the reflection of external light, compensating for color, and converting linearly polarized light into circularly polarized light. EXAMPLES

[0219] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. The resin characteristics were evaluated by the following methods. The characteristic evaluation method is not limited to the following methods, and can be appropriately selected by a person skilled in the art.

[0220] (1) Measurement of reduced viscosity A polycarbonate resin was dissolved using a solvent to prepare a polycarbonate solution with a concentration of 1.00 g / dl. A mixed solvent of phenol and 1,1,2,2-tetrachloroethane was used as the solvent. The mixing ratio of phenol to 1,1,2,2-tetrachloroethane was 1:1 by mass. Dissolution into the mixed solvent was carried out over 30 minutes while stirring at 110°C. The polycarbonate solution after cooling was used to measure the reduced viscosity. The reduced viscosity was measured at a temperature of 30.0°C ± 0.1°C using a Chuo Rika Ubbelohde viscometer "DT-504 automatic viscometer." The solvent passage time t 0 From the solution passing time t, the relative viscosity η is calculated using the following formula (α): rel Calculate the relative viscosity η rel From the following formula (β), the specific viscosity η sp (Unit: g cm -1 ·sec -1 ) was calculated. Note that η in formula (β) 0 is the viscosity of the solvent. And the specific viscosity η sp Divide by the concentration c (g / dL) of the polycarbonate solution to obtain the reduced viscosity η (η = η sp / c) was calculated. A higher value indicates a higher molecular weight. η rel =t / t 0 (α) η sp =(η - η 0 ) / η 0 = η rel -1 (β)

[0221] (2) Measurement of glass transition temperature (Tg) The glass transition temperature was measured using a differential scanning calorimeter "EXSTAR 6220" manufactured by SII Nano Technology Co., Ltd. The measurement was performed in accordance with JIS K7121:1987. Specifically, about 10 mg of the measurement sample was heated at a heating rate of 10 ° C / min, and the sample heated to 250 ° C was quenched with liquid nitrogen and heated again to 250 ° C at a heating rate of 10 ° C / min. From the DSC data obtained in the second heating, the midpoint glass transition onset temperature is calculated from the temperature at which a straight line equidistant in the vertical direction from a straight line extending the low-temperature side baseline and the high-temperature side baseline intersects with the curve of the step-like change part of the glass transition. This midpoint glass transition onset temperature is treated as the glass transition temperature Tg. Resins with high glass transition temperatures are excellent in terms of heat resistance.

[0222] (3) Press film production Polycarbonate resin pellets were vacuum dried at 90°C for 5 hours or more. A spacer was prepared by hollowing out a metal plate (SUS) with an outer width of 10 cm length, 10 cm width, and 0.5 mm thickness, leaving a width of 1 cm, and an inner width of 8 cm length and 8 cm width. This spacer was sandwiched between two mirror-finished SUS plates with a length of 10 cm length, width of 10 cm width, and thickness of 1.5 mm, and about 4 g of pellets were placed inside the spacer frame and heat pressed. The heat press temperature was 200 to 230°C, the preheating time was 5 to 7 minutes, and the pressure during molding was 40 MPa. The pressure time during molding was 1 minute. After the heat press, the sheet-like sample was taken out together with the mirror plate and spacer, and was pressurized and cooled for 3 minutes at a pressure of 20 MPa using a water tube cooling press. A film with a thickness of 400 to 500 μm was produced.

[0223] (4) Refractive index measurement From the film prepared by method (3), rectangular test pieces with a length of 10 to 20 mm and a width of 8 mm were cut out to be used as measurement samples. The refractive indices, nC, nD, ne, and nF, at each wavelength were measured using an Abbe refractometer (Atago's "DR-M4") with interference filters of wavelengths of 656 nm (C-line), 589 nm (D-line), 546 nm (e-line), and 486 nm (F-line). The measurements were performed at 20°C using 1-bromonaphthalene as the interface liquid. The Abbe number νd was calculated using the following formula: νd=(1-nD) / (nC-nF) The larger the Abbe number, the smaller the wavelength dependency of the refractive index becomes, and for example, the smaller the focal point shift due to wavelength when a single lens is used.

[0224] (5) Measurement of photoelastic coefficient The measurements were carried out as follows using a combination of a birefringence measuring device consisting of a He-Ne laser, polarizer, compensation plate, analyzer and photodetector, and a vibration type viscoelasticity measuring device (DVE-3 manufactured by Rheology Co., Ltd.) (For details, refer to the Journal of the Society of Rheology of Japan, Vol. 19, pp. 93-97 (1991).) Resins with low photoelastic coefficients have little effect on optical properties when film shape changes due to temperature or humidity changes, and are excellent in terms of performance stability against environmental conditions.

[0225] A sample with a width of 5 mm and a length of 20 mm was cut out from the film prepared by the method (3) and fixed to a viscoelasticity measuring device, and the storage modulus E' was measured at a frequency of 96 Hz at room temperature of 25°C. At the same time, the emitted laser light was passed through a polarizer, a sample, a compensation plate, and an analyzer in that order, and picked up by a photodetector (photodiode). The amplitude and phase difference with respect to the strain were obtained for the waveform of angular frequency ω or 2ω through a lock-in amplifier, and the strain optical coefficient O' was obtained. At this time, the directions of the polarizer and the analyzer were adjusted to be perpendicular to each other and to form an angle of π / 4 with respect to the stretching direction of the sample. The photoelastic coefficient C was calculated from the storage modulus E' and the strain optical coefficient O' by the following formula. C=O' / E'

[0226] (6) Saturated water absorption rate The film prepared by method (3) was cut into a shape of approximately 40 mm in length and 40 mm in width to prepare a measurement sample. The measurement test piece (film) was dried in a vacuum dryer at 90°C under vacuum for 5 hours or more, and then cooled to room temperature while maintaining the vacuum. Dry air was introduced to return the pressure to normal pressure, and the dry weight W0 of the measurement test piece (film) was quickly measured. The test piece (film) was immersed in 500cc of pure water at room temperature (23°C) and left for 96 hours. After 96 hours, the test piece (film) was taken out, the water on the surface of the test piece (film) was wiped off with a cloth, and the weight W1 after water absorption was quickly measured. The saturated water absorption rate was calculated using the following formula. Saturated water absorption rate (%)=((W1-W0) / W0)×100

[0227] (7) Boiling water test (evaluation of moist heat resistance) The film prepared by method (3) was cut into a shape of approximately 40 mm in length and 40 mm in width to prepare a measurement sample. The test piece (film) was placed in a mesh basket and immersed in a water tank heated to 100°C and left for 3 hours. After 3 hours, the mesh basket was removed and the test piece was cooled, after which the appearance of the test piece was observed. Test pieces (films) that were not deformed were rated as pass (○), and those that were deformed were rated as fail (×).

[0228] (8)Pencil hardness The pencil hardness of the film prepared by the method (3) was measured in accordance with JIS K5600-5-4:1999 using a pencil hardness tester (No. 601-B, manufactured by Mize Testing Instruments Co., Ltd.) under conditions of a load of 750 g and a measurement speed of 60 mm / min. (9) 5% thermogravimetric reduction temperature (Td5) Using a TG / DTA7200 manufactured by SII Nano Technology, approximately 10 mg of the sample was placed in a container and measured from 40°C to 500°C at a heating rate of 10°C / min under a nitrogen atmosphere (nitrogen flow rate 50 ml / min), and the temperature at which the weight decreased by 5% (Td5) was calculated. The higher this temperature, the less likely the sample is to undergo thermal decomposition. (10)NMR The measurements for Synthesis Examples 1 and 2 were performed using the solvents described in each Synthesis Example. Deuterated chloroform was used as the solvent for Synthesis Examples 3 and 4, and deuterated dimethyl sulfoxide was used as the solvent for Synthesis Examples 5 and 6. 1H-NMR was measured using an AVANCE manufactured by Bruker Biospin at a resonance frequency of 400 MHz and at room temperature. In the measurements of Examples 1, 2, 6, 10 to 16, about 30 mg of sample was placed in an NMR sample tube with an outer diameter of 5 mm and dissolved in 0.7 ml of deuterated chloroform (containing 0.03 v / v% tetramethylsilane). 1H-NMR was measured using a Bruker AVANCE III 950 at a resonance frequency of 950.3 MHz, a flip angle of 30°, and a measurement temperature of 25°C.

[0229] [Example of calculation of Tg of homopolymer] The Tg of an amorphous polymer copolymer made of various monomers can be calculated from the Flory-Fox equation based on the Tg of the homopolymer of each monomer constituting the polymer and the weight fraction of the monomer (copolymerization ratio on a weight basis). The Flory-Fox equation, as shown below, is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer. 1 / Tg=Σ(Wi / Tgi) In the Flory-Fox formula, Tg is the glass transition temperature (unit: K) of the copolymer, Wi is the weight fraction (copolymerization ratio by weight) of monomer i in the copolymer, and Tgi is the glass transition temperature (unit: K) of a homopolymer of monomer i. As the Tg of the homopolymer, a value described in a publicly known document or an actually measured value may be adopted. Using this formula, for example, if the Tg1 of the homopolymer of one monomer component M1 is known for a copolymer consisting of two monomer components M1 and M2, and the Tg of one or more copolymers with different composition ratios can be measured for a copolymer with the second component M2, the Tg2 of the homopolymer of the second component M2 can be calculated and estimated. When a copolymer is composed of two monomer components, the Flory-Fox formula is as follows. 1 / Tg=W1 / Tg1+W2 / Tg2 W1+W2=1 Here, Tg: Tg of the copolymer, Tg1: Tg of the M1 homopolymer, Tg2: Tg of the M2 homopolymer, W1: weight fraction of the M1 homopolymer component, W2: weight fraction of the M2 homopolymer component. If we transform this 1 / Tg=(1 / Tg1-1 / Tg2)W1+1 / Tg2 By using the least squares method to calculate the y-axis intercept from a graph with 1 / Tg on the y-axis and W1 on the x-axis, Tg2 can be found from that value.

[0230] [Monomer synthesis example] Synthesis of IN88;

[0231] <Synthesis Example 1-1> Synthesis of Compound 2 [ka] In a 2L four-neck flask, 125g (694mmol) of myo-inositol (1), 122g (1015mmol) of trimethyl orthoacetate, 1L of N,N-dimethylformamide, and 9.56g (55.5mmol) of p-toluenesulfonic acid were added, and the mixture was heated and stirred at an internal temperature of 100°C for 3 hours. After confirming the disappearance of the raw material myo-inositol by thin layer chromatography (hereinafter abbreviated as TLC), the reaction solution was cooled to 0°C and adjusted to pH 7 with an aqueous sodium hydroxide solution. The pH-adjusted reaction solution was concentrated under reduced pressure to remove the solvent, and then 2.5L of methanol was added to form a suspension, which was thoroughly stirred and filtered to obtain 104g (509mmol, 73% yield) of compound 2 as a white solid.

[0232] The chemical shifts of compound 2 are shown below. 1 H NMR (400MHz, DMSO-d 6 )δ=5.40(s,2H),5.20(brd,J=4.4Hz,1H),4.23(t,J=4.0Hz,2H),4.03-3.98(m,1H),3.97-3.91(m,3H),1.28(s,3H).

[0233] <Synthesis Example 1-2> Synthesis of Compound 3 [ka] In a 3L four-neck flask, 64.6g (1.62mmol) of 60% sodium hydride and 1.5L of N,N-dimethylformamide were added, and under nitrogen, compound 2 (150g, 735mmol) obtained in the same manner as in Synthesis Example 1-1 was added little by little. The reaction solution was stirred at 0°C for 30 minutes, and then 97.4g (808mmol) of pivaloyl chloride was slowly dropped into the reaction solution and stirred at 19°C for 16 hours. After confirming the disappearance of the raw material compound 2 by TLC, acetic acid was added to adjust the reaction solution to pH 7. The reaction solution was concentrated under reduced pressure and the solvent was distilled off, and then 2.5L of ethyl acetate was added and stirred thoroughly as a suspension, and the solid content was removed by filtration, and the obtained filtrate was concentrated under reduced pressure and the solvent was distilled off, and the compound 3 was purified by silica gel column chromatography to obtain 146g (506mmol, yield 69%) of white solid.

[0234] The chemical shifts of compound 3 are shown below. 1 H NMR(400MHz,DMSO-d6)δ=5.57(d,J=6.0Hz,2H),5.15(s,1H),4.35-4.22(m,2H),4.16-4.02(m,3H),1.30(s,3H),1.19(s,9H).

[0235] <Synthesis Example 1-3> Synthesis of Compound 4 [ka] Compound 3 (52.5 g, 182 mmol) obtained in the same manner as in Synthesis Example 1-2, 750 mL of toluene, 10-camphorsulfonic acid hydrate 1.14 g (4.55 mmol), and malondialdehyde bis(dimethyl acetal) 15.0 g (91.1 mmol) were added to a 2 L four-neck flask, a reflux tube filled with 4A molecular sieves was set, and the mixture was heated and stirred for 12 hours in an oil bath at 120 ° C. under nitrogen. After confirming the disappearance of the raw materials by TLC, the mixture was concentrated under reduced pressure to remove the solvent, and purified by silica gel column chromatography to obtain 53.0 g (86.5 mmol, 95% yield) of compound 4 as a gray solid.

[0236] The chemical shifts of compound 4 are shown below. 1 H NMR (400 MHz, CDCl 3 )δ=5.41-5.33(m,4H),4.91-4.87(m,2H),4.74(t,J=4.8Hz,4H),4.32-4.29(m,4H) ,1.85-1.80(m,1H),1.83(t,J=5.2Hz,2H),1.46-1.44(m,6H),1.28-1.27(m,18H).

[0237] <Synthesis Example 1-4> Synthesis of IN88 [ka] Compound 4 (53.0 g, 86.5 mmol) obtained in the same manner as in Synthesis Example 1-3, 300 mL of tetrahydrofuran, 300 mL of methanol, and 10.4 g (260 mmol) of sodium hydroxide were added to a 1L four-neck flask and stirred at 30°C for 12 hours. After confirming the disappearance of the raw materials by TLC, 300 mL of desalted water was added and the precipitated white solid was filtered. 360 mL of desalted water was added to the obtained solid, and the mixture was heated and stirred at 100°C for 4 hours, filtered, and the obtained solid was dried under reduced pressure to obtain 38.1 g (85.7 mmol, yield 99%) of IN88.

[0238] The chemical shifts of IN88 are shown below. 1 H NMR: (400MHz, DMSO-d 6 )δ=5.29(t,J=5.2Hz,2H),5.22(d,J=7.6Hz,2H),5.05(brt,J=4.8Hz,2H),4.59(t,J=4.8Hz,4H ),4.09-4.06(m,1H),4.10-4.05(m,1H),4.03-4.00(m,4H),1.59(t,J=5.2Hz,2H),1.31(s,6H). 13 C NMR (400 MHz, DMSO-d 6 )δ=107.29,88.95,72.35,65.56,61.12,58.99,24.13.

[0239] The LC-MS data for IN88 is shown below. LC-MS(ESI)m / z:445.2[M+H]

[0240] Synthesis of IN89; <Synthesis Example 2-1> Synthesis of Compound 6 [ka] In a 500 mL four-neck flask, 233 g (1.16 mol) of glutaraldehyde, 200 mL of methanol, and 4.0 g (23.3 mmol) of p-toluenesulfonic acid were added and heated and stirred at 65° C. for 96 hours. The reaction solution was concentrated under reduced pressure to give compound 6 (220 g) as a yellow oily substance, which was used in the next step without any particular purification.

[0241] <Synthesis Example 2-2> Synthesis of Compound 7 [ka] In a 1L four-neck flask, 600mL of toluene, compound 6 (22.3g, 116mmol) obtained by the same method as in Synthesis Example 2-1, compound 3 (50.0g, 173mmol) obtained by the same method as in Synthesis Example 1-2, and 2.17g (8.67mmol) of 10-camphorsulfonic acid hydrate were added, a reflux tube filled with 4A molecular sieves was set, and the mixture was heated and stirred for 2 hours in an oil bath at 120°C under nitrogen. After confirming the disappearance of the raw materials by TLC, the mixture was concentrated under reduced pressure and purified by silica gel column chromatography to obtain 26.7g (41.6mmol, 36% yield) of compound 7 as a gray solid.

[0242] The chemical shifts of compound 7 are shown below. 1 H NMR(400MHz,CHLOROFORM-d)δ=5.40(t,J=2.0Hz,2H),5.21(t,J=4.4Hz,2H),4.87(brt,J=4.4H z,2H),4.73(t,J=4.8Hz,4H),4.34-4.28(m,4H),1.58-1.49(m,4H),1.45(s,8H),1.28(s,18H).

[0243] <Synthesis Example 2-3> Synthesis example of IN89 [ka] Compound 7 (56.0 g, 87.4 mmol) obtained in the same manner as in Synthesis Example 2-1, 400 mL of methanol, 400 mL of tetrahydrofuran, and 21.0 g (524 mmol) of sodium hydroxide were added to a 2 L four-neck flask and stirred at 7-18 ° C for 40 hours. After confirming the disappearance of the raw materials by TLC, 1 L of desalted water was added to the reaction solution, and the precipitated white solid was filtered. 300 mL of desalted water was added to the obtained solid, and the mixture was heated and stirred at 100 ° C for 4 hours, and then the filtered solid was dried under reduced pressure to obtain 40.5 g (85.7 mmol, yield 98%) of IN89.

[0244] The chemical shifts of IN89 are shown below. 1 H NMR (400MHz, DMSO-d 6 )δ=5.25(t,J=4.0Hz,2H),5.20(d,J=7.6Hz,2H),5.06-4.96(m,2H),4.58(t,J=4.8Hz, 4H),4.13-4.06(m,2H),4.05-3.98(m,4H),1.39(brdd,J=4.4,7.2Hz,4H),1.31(s,8H). 13 C NMR (400 MHz, DMSO-d 6 ):107.25,91.53,72.45,65.44,61.32,58.99,33.70,24.11,17.32.

[0245] The LC-MS data for IN89 is shown below. LC-MS(ESI)m / z:473.4[M+H]

[0246] DCMI, IN44, IN45, and IN58 were synthesized as follows according to the method described in WO2016 / 098898. [Synthesis Example 3: Synthesis of DL-2,3:5,6-di-O-cyclohexylidene-myo-inositol (hereinafter abbreviated as "DCMI")] After replacing the atmosphere in a 500 ml reaction vessel equipped with a Dimroth filter with nitrogen, 30 g (167 mmol) of myo-inositol, 200 mL of DMF, 863 mg of p-toluenesulfonic acid monohydrate, and 75 mL of dimethoxycyclohexane were added and stirred at 100 ° C for 3 hours. After cooling to 40 ° C, 2.5 mL of triethylamine was added, and the reaction solvent DMF was distilled off under reduced pressure. Then, 250 mL of ethyl acetate was added, and the mixture was separated with 300 mL of 5% aqueous sodium carbonate solution, and washed once with 300 mL of ion-exchanged water. The organic phase obtained was distilled off under reduced pressure, and crystallization was performed with 50 mL of ethyl acetate / 70 mL of n-hexane, and the obtained white precipitate was filtered. Then, crystallization was performed again with 50 mL of ethyl acetate / 70 mL of n-hexane. The obtained solid was vacuum dried at 60 ° C for 5 hours to obtain 9.8 g of the target compound DCMI (yield 17.2%). 1H-NMR analysis of this compound confirmed that it was the target compound, and gas chromatographic analysis confirmed that it was 99.0 area %.

[0247] [Synthesis Example 4: Synthesis of DL-2-O-benzyl-1,3,5-O-ethylidene-myo-inositol (hereinafter abbreviated as IN44)]

[0248] (Synthesis Example 4-1) Synthesis of DL-1,3,5-O-ethylidene-myo-inositol (hereinafter abbreviated as OEM) After replacing the atmosphere in a reaction vessel equipped with a Dimroth and Dean-Stark tube with nitrogen, 140 g (777 mmol) of myo-inositol, 582 g of DMF, 11.8 g (62.2 mmol) of p-toluenesulfonic acid monohydrate, and 135 g (1127 mmol) of trimethyl orthoacetate were added, and the mixture was immersed in an oil bath at 130°C and stirred for 40 minutes. During this time, the liquid that had distilled off into the Dean-Stark tube was removed. After cooling to room temperature, 93.7 g of a 6.2 wt% aqueous solution of sodium bicarbonate was added, and the DMF was distilled off under reduced pressure. Then, 300 mL of methanol was added to the resulting concentrate, which was dissolved by heating, cooled, crystallized, and filtered. The resulting solid was After vacuum drying at 50°C for 8 hours, 117.5g (74% yield) of the target compound OEM was obtained. 1H-NMR analysis of this compound confirmed that it was the target compound.

[0249] (Synthesis Example 4-2) Synthesis of DL-2-O-benzyl-1,3,5-O-ethylidene-myo-inositol (hereinafter abbreviated as IN44) After replacing the atmosphere in a 1000mL reaction vessel with nitrogen, 15.67g (391.8mmol) of 60% by weight sodium hydride and 360mL of DMF were added, and a solution in which 80g (381.8mmol) of OEM synthesized in Synthesis Example 8-1 was dissolved in 360mL of DMF was added dropwise. Then, 67.02g (391.8mmol) of benzyl bromide was added dropwise to the reaction vessel, and the mixture was stirred for 1 hour at an internal temperature of 10 to 25°C. Then, 80g of ion-exchanged water was added, and DMF was distilled off under reduced pressure. Extraction was performed by adding 400mL of ethyl acetate and 300mL of ion-exchanged water, and the organic layer was recovered. Next, 300mL of ion-exchanged water was added for washing, and the organic layer was recovered by separation. Furthermore, 300mL of ion-exchanged water was added for washing, and the organic layer was recovered by separation. After ethyl acetate was distilled off under reduced pressure, 120 mL of methanol and 100 mL of heptane were added and stirred, and then the mixture was separated to recover the methanol layer. After methanol was distilled off under reduced pressure, 100 mL of tert-butyl methyl ether was added to perform crystallization, and the resulting white solid was collected by filtration. Furthermore, the resulting white solid was recrystallized with 80 mL of ethyl acetate and 80 mL of heptane, and the resulting white solid was collected by filtration. The resulting solid was vacuum dried at 50°C for 8 hours to obtain 60 g (yield 52%) of the target compound IN44. 1H-NMR analysis of this compound confirmed that it was the target compound, and gas chromatographic analysis confirmed that it was 99.7 area %.

[0250] [Synthesis Example 5: Synthesis of DL-2-O-benzyl-1,3,5-O-methylidene-myo-inositol (hereinafter abbreviated as IN45)] (Synthesis Example 5-1) Synthesis of DL-1,3,5-O-methylidene-myo-inositol (hereinafter abbreviated as OEH) After replacing the atmosphere in a reaction vessel equipped with a Dimroth tube and a Dean-Stark tube with nitrogen, 134.76 g (748.0 mmol) of myo-inositol, 560 g of DMF, 11.38 g (59.8 mmol) of p-toluenesulfonic acid monohydrate, and 111.13 g (1047.2 mmol) of trimethyl orthoformate were added, and the mixture was stirred for 5 hours in an oil bath at 130°C. During this time, the liquid that had distilled off into the Dean-Stark tube was removed. After cooling to room temperature, 72 g of a 7.7 wt% aqueous solution of sodium bicarbonate was added, and the DMF was distilled off under reduced pressure. Then, 500 mL of methanol was added to the resulting concentrate, which was dissolved by heating, cooled, crystallized, and filtered. The resulting solid was vacuum dried at 50°C for 8 hours, yielding 63.3 g (45% yield) of the target compound, OEH. This compound was analyzed by 1H-NMR and confirmed to be the target compound.

[0251] (Synthesis Example 5-2) Synthesis of DL-2-O-benzyl-1,3,5-O-methylidene-myo-inositol (hereinafter abbreviated as IN45) After replacing the atmosphere in a 200mL reaction vessel with nitrogen, 2.73g (68.4mmol) of 60% by weight sodium hydride and 65mL of DMF were added, and a solution in which 13g (68.4mmol) of OEH synthesized in Synthesis Example 9-1 was dissolved in 65mL of DMF was dropped. Then, 11.69g (68.4mmol) of benzyl bromide was dropped into the reaction vessel, and the mixture was stirred for 1 hour at an internal temperature of 9 to 12°C. Then, 30g of ion-exchanged water was added, and DMF was distilled off under reduced pressure. 100mL of ethyl acetate and 100g of ion-exchanged water were added to the concentrate to perform extraction, and the organic layer was recovered. Furthermore, 100g of ion-exchanged water was added for washing, and the organic layer was recovered by separation. After distilling off the ethyl acetate under reduced pressure, 50mL of methanol and 50mL of heptane were added and stirred, and the mixture was separated to recover the methanol layer, and the methanol was distilled off under reduced pressure. The concentrate was crystallized by adding 60 mL of tert-butyl methyl ether, and the resulting white solid was collected by filtration. The resulting white solid was recrystallized with 40 mL of ethyl acetate and 40 mL of heptane, and the resulting white solid was collected by filtration. The resulting solid was vacuum dried at 50°C for 8 hours, and 10.9 g (yield 57%) of the target compound IN45 was obtained. 1H-NMR analysis of this compound confirmed that it was the target compound, and gas chromatographic analysis confirmed that it was 99.8 area %.

[0252] [Synthesis Example 6: Synthesis of DL-2-O-cyclohexylmethyl-1,3,5-O-ethylidene-myo-inositol (hereinafter abbreviated as IN58)] After replacing the atmosphere in a 1000mL reaction vessel with nitrogen, 14.7g (3367.3mmol) of 60% by weight sodium hydride and 320mL of DMF were added, and a solution in which 75g (367.3mmol) of OEM synthesized in Synthesis Example 8-1 was dissolved in 360mL of DMF was added dropwise. Then, 65.05g (367.3mmol) of cyclohexylmethyl bromide was added dropwise to the reaction vessel, and the mixture was stirred for 2 hours at an internal temperature of 80 to 90°C. After cooling to room temperature, 14.7g (3367.3mmol) of 60% by weight sodium hydride was added, and the mixture was stirred at room temperature for 30 minutes, and then, 65.05g (367.3mmol) of cyclohexylmethyl bromide was added dropwise to the reaction vessel, and the mixture was stirred for 2 hours at an internal temperature of 80 to 90°C. After cooling to room temperature, 90g of ion-exchanged water was added, and the DMF was distilled off under reduced pressure. Extraction was performed by adding 400 mL of ethyl acetate and 300 g of ion-exchanged water, and the organic layer was collected. Next, 300 g of ion-exchanged water was added and washed, and then the organic layer was collected by separation. Furthermore, 300 g of ion-exchanged water was added and washed, and then the organic layer was collected by separation. After ethyl acetate was distilled off under reduced pressure, 200 mL of methanol and 100 mL of n-hexane were added and stirred, and then the methanol layer was collected by separation. After methanol was distilled off under reduced pressure, 50 mL of tert-butyl methyl ether and 100 mL of n-hexane were added to perform recrystallization, and the obtained white solid was collected by filtration. Furthermore, the obtained white solid was crystallized with 100 mL of tert-butyl methyl ether and 100 mL of n-hexane, and the obtained white solid was collected by filtration. The obtained solid was vacuum dried at 50 ° C for 8 hours, and 29 g (yield 26%) of the target compound IN58 was obtained. 1H-NMR analysis of this compound was performed to confirm that it was the target compound, and gas chromatographic analysis was performed to confirm that it was 99.4 area %.

[0253] [Synthesis example of polycarbonate resin and characteristic evaluation] The abbreviations of the compounds used in the following Examples and Comparative Examples are as follows. DCMI: DL-2,3:5,6-di-O-cyclohexylidene-myo-inositol ISB: Isosorbide (manufactured by Rocket Fleuret, product name: POLYSORB) CHDM: 1,4-cyclohexanedimethanol (cis-trans mixture, manufactured by SK Chemicals) TCDDM: Tricyclodecane dimethanol [Oxea] SPG: Spiroglycol (manufactured by Mitsubishi Gas Chemical Co., Ltd.) 1,6-Hexanediol (1,6-HD) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 1,10-Decanediol (1,10-DD) (Tokyo Chemical Industry Co., Ltd.) BPEF: 9,9-bis[4-(2-hydroxyethoxy)phenyl]-fluorene (Osaka Gas Chemicals Co., Ltd.) DPC: Diphenyl carbonate (Mitsubishi Chemical)

[0254] [Example 1] 5.77 g (0.0130 mol) of IN88, 4.74 g (0.0324 mol) of isosorbide (hereinafter abbreviated as "ISB"), 2.81 g (0.0195 mol) of 1,4-cyclohexanedimethanol (hereinafter abbreviated as "CHDM"), 14.18 g (0.0662 mol) of diphenyl carbonate (hereinafter abbreviated as "DPC"), and 1.14 × 10 calcium acetate monohydrate as a catalyst. -3 g (6.49 × 10 -6 The raw materials were charged into a reaction vessel as a 0.2% by mass aqueous solution, and the heating vessel was heated to 150°C under a nitrogen atmosphere. Stirring was performed as necessary, and the temperature was raised to 220°C in 60 minutes at normal pressure to dissolve the raw materials. In the first step of the reaction, the temperature was kept at 220°C, and the pressure was reduced from normal pressure to 13.3 kPa in 40 minutes, and then the pressure was kept at 13.3 kPa for 60 minutes, and the generated phenol was discharged outside the reaction vessel. In the second step, the heating tank temperature was increased to 240°C in 20 minutes, and the generated phenol was discharged outside the reaction vessel while controlling the pressure to be 0.200 kPa or less in 30 minutes. After reaching a predetermined stirring torque, the reaction was terminated, and the generated reaction product was removed from the reaction vessel to obtain a polycarbonate copolymer. The reduced viscosity of the obtained polycarbonate copolymer was 0.547 dl / g, and the glass transition temperature Tg was 179°C. The 5% thermal weight loss temperature Td5 was 351°C. The refractive indices measured at 20°C were nC = 1.502, nD = 1.504, ne = 1.507, and nF = 1.513, and the Abbe number νD was 46. The photoelastic coefficient was 11×10 -12 Pa -1 The saturated water absorption was 3.0%, and the boiling water test was passed without any deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 1. The above-mentioned various evaluations were carried out using the obtained polycarbonate resin pellets. The evaluation results are shown in the table below.

[0255] [Example 2] 3.31 g (0.0074 mol) of IN88, 6.53 g (0.0447 mol) of ISB, 3.22 g (0.0223 mol) of CHDM, 16.28 g (0.0760 mol) of DPC, and 3.28 × 10 calcium acetate monohydrate as a catalyst. -4 g (1.86 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.756 dl / g, and the glass transition temperature Tg was 158°C. The 5% thermal weight loss temperature Td5 was 345°C. The refractive indexes measured at 20°C were nC = 1.517, nD = 1.519, ne = 1.522, and nF = 1.527, and the Abbe number νD was 52. The saturated water absorption was 2.5%, and the boiling water test was passed without deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 2.

[0256] [Example 3] 5.37 g (0.0121 mol) of IN88, 8.59 g (0.0282 mol) of spiroglycol (hereinafter abbreviated as "SPG"), 8.80 g (0.0411 mol) of DPC, and 7.10 x 10 calcium acetate monohydrate as a catalyst. -4 g (4.03 × 10 -6A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.477 dl / g and a glass transition temperature Tg of 150° C. The 5% thermal weight loss temperature Td5 was 399° C.

[0257] [Example 4] 8.26 g (0.0186 mol) of IN88, 5.13 g (0.0434 mol) of 1,6-hexanediol (hereinafter abbreviated as "1,6-HD"), 13.54 g (0.0632 mol) of DPC, and 1.09 × 10 calcium acetate monohydrate as a catalyst. -3 g(6.20×10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.408 dl / g and a glass transition temperature Tg of 88°C.

[0258] [Example 5] 9.94 g (0.0224 mol) of IN88, 3.90 g (0.0224 mol) of 1,10-decanediol (hereinafter abbreviated as "1,10-DD"), 9.77 g (0.0456 mol) of DPC, and 7.88 × 10 calcium acetate monohydrate as a catalyst. -3 g (4.47 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.378 dl / g and a glass transition temperature Tg of 104°C.

[0259] [Example 6] 7.68 g (0.0173 mol) of IN88, 5.82 g (0.0404 mol) of CHDM, 12.59 g (0.0588 mol) of DPC, and 1.02 × 10 calcium acetate monohydrate as a catalyst. -3 g(5.77×10 -6A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.555 dl / g, and the glass transition temperature Tg was 155°C. The 5% thermal weight loss temperature Td5 was 357°C. The refractive indexes measured at 20°C were nC = 1.509, nD = 1.513, ne = 1.515, and nF = 1.522, and the Abbe number νD was 39. The saturated water absorption was 1.5%, and the boiling water test was passed without deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 3.

[0260] [Example 7] 6.80 g (0.0153 mol) of IN88, 6.62 g (0.0459 mol) of CHDM, 13.36 g (0.0624 mol) of DPC, and 2.70 × 10 calcium acetate monohydrate as a catalyst. -4 g (1.53 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.720 dl / g, and the glass transition temperature Tg was 141°C. The 5% thermal weight loss temperature Td5 was 357°C. The refractive indexes measured at 20°C were nC = 1.500, nD = 1.503, ne = 1.505, and nF = 1.510, and the Abbe number νD was 50. The saturated water absorption was 1.4%, and the boiling water test was passed without deformation. The pencil hardness was 2H.

[0261] [Example 8] 5.79 g (0.0130 mol) of IN88, 7.52 g (0.0521 mol) of CHDM, 14.52 g (0.0678 mol) of DPC, and 2.86 × 10 calcium acetate monohydrate as a catalyst. -4 g (1.62 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.963 dl / g, and the glass transition temperature Tg was 127° C. The 5% thermal weight loss temperature Td5 was 358° C. The saturated water absorption was 1.1%, and the boiling water test was passed without any deformation.

[0262] [Example 9] 5.86 g (0.0153 mol) of IN88, 7.77 g (0.0459 mol) of tricyclodecane dimethanol (hereinafter abbreviated as "TCDDM"), 11.53 g (0.0624 mol) of DPC, and 2.32 × 10 calcium acetate monohydrate as a catalyst. -4 g (1.32 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.501 dl / g, and the glass transition temperature Tg was 144°C. The 5% thermal weight loss temperature Td5 was 364°C. The refractive indexes measured at 20°C were nC = 1.520, nD = 1.522, ne = 1.525, and nF = 1.530, and the Abbe number νD was 52. The saturated water absorption was 0.9%, and the boiling water test was passed without deformation. The pencil hardness was 2H.

[0263] [Example 10] 2.86 g (0.0064 mol) of IN88, 11.30 g (0.0258 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter abbreviated as “BPEF”), 7.04 g (0.0329 mol) of DPC, and 5.68×10 calcium acetate monohydrate as a catalyst. -4 g(3.22×10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.740 dl / g and a glass transition temperature Tg of 175° C. The 5% thermal weight loss temperature Td5 was 381° C. The NMR spectrum of this polycarbonate copolymer is shown in FIG.

[0264] [Example 11] 3.47 g (0.0073 mol) of IN89, 6.44 g (0.0441 mol) of ISB, 3.18 g (0.0221 mol) of CHDM, 16.05 g (0.0749 mol) of diphenyl carbonate (hereinafter abbreviated as "DPC"), and 1.29 × 10 calcium acetate monohydrate as a catalyst. -3 g (7.34 × 10 -6 The raw materials were charged into a reaction vessel as a 0.2% by mass aqueous solution, and the heating vessel was heated to 150°C under a nitrogen atmosphere. Stirring was performed as necessary, and the temperature was raised to 220°C in 60 minutes at normal pressure to dissolve the raw materials. In the first step of the reaction, the temperature was kept at 220°C, and the pressure was reduced from normal pressure to 13.3 kPa in 40 minutes, and then the pressure was kept at 13.3 kPa for 60 minutes, and the generated phenol was discharged outside the reaction vessel. In the second step, the heating tank temperature was increased to 240°C in 20 minutes, and the generated phenol was discharged outside the reaction vessel while controlling the pressure to be 0.200 kPa or less in 30 minutes. After reaching a predetermined stirring torque, the reaction was terminated, and the generated reaction product was removed from the reaction vessel to obtain a polycarbonate copolymer. The reduced viscosity of the obtained polycarbonate copolymer was 0.687 dl / g, and the glass transition temperature Tg was 148°C. The 5% thermal weight loss temperature Td5 was 348°C. The refractive indices measured at 20°C were nC = 1.516, nD = 1.518, ne = 1.522, and nF = 1.526, and the Abbe number νD was 52. The photoelastic coefficient was 15×10 -12 Pa -1 The saturated water absorption was 2.4%, and the boiling water test was passed without any deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 5.

[0265] [Example 12] 6.01 g (0.0129 mol) of IN89, 7.34 g (0.0509 mol) of CHDM, 13.90 g (0.0649 mol) of DPC, and 1.12 × 10 calcium acetate monohydrate as a catalyst. -3 g (6.36×10 -6A polycarbonate copolymer was obtained in the same manner as in Example 11 except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.572 dl / g, and the glass transition temperature Tg was 110°C. The 5% thermal weight loss temperature Td5 was 360°C. The saturated water absorption was 0.9%, and the boiling water test was passed without any deformation. The pencil hardness was H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 6.

[0266] [Example 13] 7.91 g (0.0167 mol) of IN89, 5.64 g (0.0391 mol) of CHDM, 12.20 g (0.0570 mol) of DPC, and 9.84 × 10 calcium acetate monohydrate as a catalyst. -4 g(5.59×10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 11 except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.779 dl / g, and the glass transition temperature Tg was 136°C. The 5% thermal weight loss temperature Td5 was 360°C. The saturated water absorption was 1.3%, and the boiling water test was passed without any deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 7.

[0267] [Example 14] 5.11 g (0.0108 mol) of IN89, 8.49 g (0.0433 mol) of TCDDM, 11.186 g (0.0551 mol) of DPC, and 9.52 × 10 calcium acetate monohydrate as a catalyst. -4 g(5.40×10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 11 except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer was 0.739 dl / g, and the glass transition temperature Tg was 120°C. The 5% thermal weight loss temperature Td5 was 366°C. The saturated water absorption was 0.7%, and the boiling water test was passed without any deformation. The pencil hardness was 2H. The NMR spectrum of this polycarbonate copolymer is shown in Figure 8.

[0268] [Example 15] 1.65 g (0.0037 mol) of IN88, 6.52 g (0.0149 mol) of BPEF, 9.53 g (0.0149 mol) of 2Q, 0.8 g (0.0037 mol) of DPC, and 3.30 × 10 calcium acetate monohydrate as a catalyst. -2 g (1.87 × 10 -4 The raw materials were charged into a reaction vessel as a 2% by mass aqueous solution, and the heating vessel was heated to 150°C under a nitrogen atmosphere. Stirring was performed as necessary, and the temperature was raised to 220°C in 60 minutes at normal pressure to dissolve the raw materials. In the first step of the reaction, the temperature was kept at 220°C, and the pressure was reduced from normal pressure to 13.3 kPa in 40 minutes, and then the pressure was kept at 13.3 kPa for 60 minutes, and the generated phenol was discharged outside the reaction vessel. In the second step, the heating tank temperature was increased to 240°C in 20 minutes, and the generated phenol was discharged outside the reaction vessel while controlling the pressure to be 0.200 kPa or less in 30 minutes. After reaching a predetermined stirring torque, the reaction was terminated, and the generated reaction product was removed from the reaction vessel to obtain a polyester carbonate copolymer. The resulting polyester carbonate copolymer had a reduced viscosity of 0.289 dl / g and a glass transition temperature Tg of 154° C. The 5% thermal weight loss temperature Td5 was 396° C. The pencil hardness was H. The NMR spectrum of this polycarbonate copolymer is shown in FIG.

[0269] [Example 16] 2.22 g (0.0050 mol) of IN88, 4.38 g (0.0300 mol) of ISB, 4.56 g (0.0150 mol) of SPG, 3.84 g (0.0060 mol) of 2Q, 9.51 g (0.0444 mol) of DPC, and 6.60 × 10 calcium acetate monohydrate as a catalyst.-3 g(3.75×10 -3 A polyester carbonate copolymer was obtained in the same manner as in Example 15, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polyester carbonate copolymer had a reduced viscosity of 0.562 dl / g and a glass transition temperature Tg of 155° C. The 5% thermal weight loss temperature Td5 was 364° C. The pencil hardness was H. The NMR spectrum of this polycarbonate copolymer is shown in FIG.

[0270] [Comparative Example 1] DCMI 4.85g (0.0142 mol), ISB 5.21g (0.0357 mol), CHDM 3.08g (0.0214 mol), DPC 15.89g (0.0742 mol), and calcium acetate monohydrate 3.14 x 10 -4 g (1.78 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.392 dl / g and a glass transition temperature Tg of 141° C. The 5% thermal weight loss temperature Td5 was 336° C.

[0271] [Comparative Example 2] DCMI 6.69 g (0.0197 mol), CHDM 6.61 g (0.0458 mol), DPC 14.59 g (0.0681 mol), and sodium bicarbonate 5.50 × 10 -5 g(6.55×10 -7 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.390 dl / g and a glass transition temperature Tg of 105° C. The 5% thermal weight loss temperature Td5 was 319° C.

[0272] [Comparative Example 3] DCMI 5.77 g (0.0170 mol), TCDDM 7.76 g (0.0395 mol), DPC 12.35 g (0.0577 mol), and calcium acetate monohydrate 5.00 × 10 -5 g (2.84 × 10 -7 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.275 dl / g and a glass transition temperature Tg of 100°C.

[0273] [Comparative Example 4] 4.88 g (0.0143 mol) of DCMI, 4.37 g (0.0144 mol) of SPG, 6.40 g (0.0299 mol) of DPC, and 6.02 × 10 calcium acetate monohydrate as a catalyst. -5 g (3.42 × 10 -7 A polycarbonate copolymer was obtained in the same manner as in Example 1 except that a 0.2 mass % aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel and the final temperature was set to 250° C. The resulting polycarbonate copolymer had a reduced viscosity of 0.201 dl / g and a glass transition temperature Tg of 136° C. The 5% thermal weight loss temperature Td5 was 346° C.

[0274] [Comparative Example 5] 3.52 g (0.0103 mol) of DCMI, 10.58 g (0.0241 mol) of BPEF, 7.46 g (0.0348 mol) of DPC, and 1.44 × 10 calcium acetate monohydrate as a catalyst. -5 g (8.17 × 10 -8 A polycarbonate copolymer was obtained in the same manner as in Example 1 except that a 0.2 mass % aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel and the final temperature was set to 250° C. The resulting polycarbonate copolymer had a reduced viscosity of 0.337 dl / g and a glass transition temperature Tg of 166° C. The 5% thermal weight loss temperature Td5 was 358° C.

[0275] [Comparative Example 6] DCMI 6.01 g (0.0177 mol), 1,10-DD 3.08 g (0.0177 mol), DPC 7.64 g (0.0357 mol), and calcium acetate monohydrate 1.56 × 10 -4 g (8.83 × 10 -7 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.742 dl / g and a glass transition temperature Tg of 72° C. The 5% thermal weight loss temperature Td5 was 330° C.

[0276] [Comparative Example 7] DCMI 7.26 g (0.0213 mol), 1,6-HD 5.89 g (0.0498 mol), DPC 15.40 g (0.0719 mol), and calcium acetate monohydrate 3.13 × 10 -4 g (1.78 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The reduced viscosity of the obtained polycarbonate copolymer could not be measured because it was insoluble in a solvent. The glass transition temperature Tg was 47°C. The 5% thermal weight loss temperature Td5 was 332°C.

[0277] [Comparative Example 8] 3.41 g (0.0116 mol) of IN44, 7.91 g (0.0541 mol) of ISB, 1.67 g (0.0116 mol) of CHDM, 17.22 g (0.0804 mol) of DPC, and 1.70 × 10 calcium acetate monohydrate as a catalyst. -3 g (9.66×10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.389 dl / g and a glass transition temperature Tg of 147° C. The 5% thermal weight loss temperature Td5 was 349° C.

[0278] [Comparative Example 9] 3.29 g (0.0117 mol) of IN45, 7.99 g (0.0547 mol) of ISB, 1.69 g (0.0117 mol) of CHDM, 17.41 g (0.0813 mol) of DPC, and 1.72 × 10 calcium acetate monohydrate as a catalyst. -3 g (9.77 × 10 -6 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 0.2% by mass aqueous solution of 1,2-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.537 dl / g and a glass transition temperature Tg of 149° C. The 5% thermal weight loss temperature Td5 was 348° C.

[0279] [Comparative Example 10] 10.249 g (0.0341 mol) of IN58, 3.28 g (0.0227 mol) of CHDM, 12.42 g (0.0580 mol) of DPC, and 1.71 x 10 calcium acetate monohydrate as a catalyst. -3 g (1.71 × 10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.393 dl / g and a glass transition temperature Tg of 143° C. The 5% thermal weight loss temperature Td5 was 367° C.

[0280] [Comparative Example 11] 89.44 g (0.612 mol) of ISB, 37.63 g (0.262 mol) of CHDM, 191.05 g (0.892 mol) of DPC, and 3.85×10 calcium acetate monohydrate as a catalyst. -3 g (2.19 × 10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.615 dl / g and a glass transition temperature Tg of 121°C.

[0281] [Comparative Example 12] 81.98 g (0.561 mol) of ISB, 47.19 g (0.240 mol) of TCDDM, 175.10 g (0.817 mol) of DPC, and 3.53 × 10 calcium acetate monohydrate as a catalyst. -3 g(2.00×10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.602 dl / g and a glass transition temperature Tg of 131°C.

[0282] [Table 1]

[0283] [Table 2]

[0284] [Table 3]

[0285] [Table 4]

[0286] [Table 5]

[0287] As can be seen from Tables 1 to 5, the thermoplastic resin having the structural unit A is excellent in heat resistance, optical properties, mechanical properties, low water absorption, and moist heat resistance in a well-balanced manner. For example, comparing Example 1 with Comparative Example 1, it is found that the thermoplastic resin having the structural unit A in Example 1 has a significantly high Tg, even though the content ratios of each structural unit are close. In addition, Comparative Examples 1 to 10 are thermoplastic resins having a structural unit derived from an inositol derivative, but do not have the structural unit B or the structural unit C, which are partial structures of the structural unit A, and therefore are inferior in heat resistance to the thermoplastic resin having the structural unit A.

[0288] [Reference example 1] ISB 127.35 g (0.612 mol), DPC 190.40 g (0.892 mol), and calcium acetate monohydrate 3.84 × 10 -3 g (2.18 × 10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1 except that a 2% by mass aqueous solution of 2-(2-methyl-1,2-diphenyl-2-propanediol) was added to the reaction vessel and the final temperature was set to 250°C. The resulting polycarbonate copolymer had a reduced viscosity of 0.538 dl / g and a glass transition temperature Tg of 164°C.

[0289] [Reference example 2] ISB 102.11 g (0.699 mol), CHDM 25.19 g (0.175 mol), DPC 190.83 g (0.891 mol), and calcium acetate monohydrate 3.85 × 10 -3 g (2.18 × 10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.585 dl / g and a glass transition temperature Tg of 133°C.

[0290] [Reference example 3] 64.03 g (0.699 mol) of ISB, 63.199 g (0.175 mol) of CHDM, 191.48 g (0.891 mol) of DPC, and 3.86 x 10 calcium acetate monohydrate as a catalyst.-3 g (2.19 × 10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.605 dl / g and a glass transition temperature Tg of 100°C.

[0291] [Reference example 4] 38.51 g (0.264 mol) of ISB, 88.66 g (0.615 mol) of CHDM, 191.91 g (0.896 mol) of DPC, and 3.87 × 10 calcium acetate monohydrate as a catalyst. -3 g(2.20×10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1, except that a 2% by mass aqueous solution of 2,4-dichlorophenyl ether (mol) was charged into the reaction vessel. The resulting polycarbonate copolymer had a reduced viscosity of 0.566 dl / g and a glass transition temperature Tg of 74°C.

[0292] [Reference example 5] 127.09 g (0.881 mol) of CHDM, 192.56 g (0.899 mol) of DPC, and 3.88 × 10 calcium acetate monohydrate as a catalyst. -3 g(2.20×10 -5 A polycarbonate copolymer was obtained in the same manner as in Example 1 except that a 2% by mass aqueous solution of 210° C. was added to the reaction vessel, the first step temperature was 210° C., and the final temperature was 210° C. The resulting polycarbonate copolymer had a reduced viscosity of 0.405 dl / g and a glass transition temperature Tg of 40°C.

[0293] The glass transition temperatures of homopolycarbonates estimated based on the Flory-Fox equation are shown in Table 6. [Calculation example 1] The glass transition temperature of the IN88 homopolycarbonate was estimated based on the Flory-Fox equation and the data of Examples 6 to 8 and Reference Example 5. The calculated value was 361°C.

[0294] [Calculation example 2] The glass transition temperature of the IN89 homopolycarbonate was estimated based on the Flory-Fox equation and the data of Examples 12, 13, and Reference Example 5. The calculated value was 271°C.

[0295] [Calculation example 3] Based on the Flory-Fox equation, the glass transition temperature of the ISB homopolycarbonate was estimated based on the data of Comparative Example 11 and Reference Examples 2 to 5. The calculated value was 169°C. In fact, the glass transition temperature of the ISB homopolycarbonate produced in Reference Example 1 was measured, and the actual value was 164°C. The calculated value and the actual value are in good agreement, and it is understood that the glass transition temperature of the homopolycarbonate can be accurately estimated based on the Flory-Fox equation.

[0296] [Calculation example 4] Based on the Flory-Fox equation, the glass transition temperature of the DCMI homopolycarbonate was estimated in the same manner as in Calculation Example 1. The calculated value was 250°C.

[0297] [Calculation example 5] Based on the Flory-Fox equation, the glass transition temperature of the IN44 homopolycarbonate was estimated in the same manner as in Calculation Example 1. The calculated value was 177°C.

[0298] [Calculation example 6] Based on the Flory-Fox equation, the glass transition temperature of the IN45 homopolycarbonate was estimated in the same manner as in Calculation Example 1. The calculated value was 178°C.

[0299] In Table 6, the weight proportion of the structural unit derived from each monomer was calculated as a repeating structural unit containing one carbonyl group (linking group).

[0300] [Table 6]

[0301] [Table 7]

[0302] As can be seen from Tables 6 and 7, the calculated Tg values ​​of the homopolycarbonates of thermoplastic resins having the structural unit A are significantly higher than the calculated Tg values ​​of the homopolycarbonates of thermoplastic resins not having the structural unit A. It is presumed that the homopolycarbonates of thermoplastic resins having the structural unit A have extremely excellent heat resistance. As can be seen from the present disclosure, inositol is a polyhydric alcohol having six hydroxyl groups, but higher-order cyclic compounds are derived depending on the configuration and bonding of the hydroxyl groups. As a result, it is found that a dihydroxy compound exhibiting extremely high heat resistance is derived. By appropriately selecting the derived dihydroxy compound, it is possible to control the physical properties of thermoplastic resins such as polycarbonate resins, such as heat resistance, water absorption, and moist heat resistance. Thus, it is found that inositol has a wide range of applicability as a natural monomer raw material.

Claims

1. A thermoplastic resin containing a structural unit A represented by the following formula (1) in the molecule, wherein X in the formula (1) is a structure represented by the following formula (3). 【Chemistry 1】 【Chemistry 2】 (In the above formula (3), R 3 , R 4 each independently represents a hydrogen atom or an organic group; Z represents a divalent organic group, and * in the formula (3) represents a bonding site.

2. The thermoplastic resin according to claim 1 , wherein in the formula (3), Z is a divalent hydrocarbon group.

3. The thermoplastic resin according to claim 1 or 2, wherein in the formula (3), Z is a divalent hydrocarbon group having 1 to 6 carbon atoms.

4. In the formula (3), R 3 , R 4 are each independently a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. The thermoplastic resin according to any one of claims 1 to 3.

5. The thermoplastic resin according to any one of claims 1 to 4, wherein the formula (3) is the following formula (4) or the following formula (5): 【Chemistry 3】 【Chemistry 4】 (In the formulas (4) and (5), * indicates a binding site.)

6. The thermoplastic resin according to claim 1 , which has a glass transition temperature of 100° C. or more and 200° C. or less.

7. The thermoplastic resin according to any one of claims 1 to 6, wherein the structural unit represented by formula (1) is contained in an amount of 1 wt% or more and 99 wt% or less when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt%.

8. The thermoplastic resin according to any one of claims 1 to 7, further comprising a structural unit derived from at least one dihydroxy compound selected from the group consisting of an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, a heteroalicyclic dihydroxy compound, and an aromatic dihydroxy compound.

9. 9. The thermoplastic resin according to claim 8, wherein the thermoplastic resin contains 1% by weight or more and 95% by weight or less of a structural unit (excluding the structural unit A) derived from at least one dihydroxy compound selected from the group consisting of an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, and a heteroalicyclic dihydroxy compound, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100% by weight.

10. The thermoplastic resin according to claim 8 or 9, comprising at least one of a structural unit derived from the alicyclic dihydroxy compound and a structural unit derived from the heteroalicyclic dihydroxy compound, and a structural unit represented by the formula (1).

11. The thermoplastic resin according to any one of claims 1 to 10, further comprising a structural unit derived from at least one dicarboxylic acid compound selected from the group consisting of an aliphatic dicarboxylic acid compound, an alicyclic dicarboxylic acid compound, a heteroalicyclic dicarboxylic acid compound, and an aromatic dicarboxylic acid compound.

12. The thermoplastic resin according to any one of claims 1 to 11, wherein the thermoplastic resin contains a structural unit represented by the following formula (6) in an amount of 1 wt% or more and 95 wt% or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt%: 【Chemistry 5】

13. The thermoplastic resin according to any one of claims 1 to 12, comprising a structural unit represented by the following formula (7) in an amount of 1 wt% or more and 95 wt% or less, when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt%: 【Chemistry 6】 (In the above formula (7), R 21 ~R 24 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.

14. The thermoplastic resin according to any one of claims 1 to 13, comprising at least one structural unit selected from the following formulas (8) to (10) in an amount of 1 wt% to 70 wt% when the total weight of all structural units and linking groups constituting the thermoplastic resin is taken as 100 wt%: 【Chemistry 7】 (In the above formula (8), R 5 ~R 8 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 6 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; X represents a substituted or unsubstituted alkylene group having 2 to 10 carbon atoms, a substituted or unsubstituted cycloalkylene group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms; and m and n each independently represent an integer of 0 to 5. 【Chemistry 8】 【Chemistry 9】 (In the formula (9) and the formula (10), R 9 ~R 11 each independently represents a direct bond or an alkylene group having 1 to 4 carbon atoms which may have a substituent, R 12 ~R 17 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an aryl group having 4 to 10 carbon atoms which may have a substituent, an acyl group having 1 to 10 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an aryloxy group having 1 to 10 carbon atoms which may have a substituent, an acyloxy group having 1 to 10 carbon atoms which may have a substituent, an amino group which may have a substituent, a vinyl group having 1 to 10 carbon atoms which may have a substituent, an ethynyl group having 1 to 10 carbon atoms which may have a substituent, a sulfur atom which has a substituent, a silicon atom which has a substituent, a halogen atom, a nitro group, or a cyano group, provided that R 12 ~R 17 At least two adjacent groups among these may be bonded to each other to form a ring.)

15. 15. The thermoplastic resin according to any one of claims 1 to 14, which is a polycarbonate or a polyester carbonate.

16. A dihydroxy compound represented by the following formula (12): 【Chemistry 10】 (In the formula (12), R 3 , R 4 each independently represents a hydrogen atom or an organic group, and Z represents a divalent organic group.

17. The dihydroxy compound according to claim 16, wherein in the formula (12), Z is a divalent hydrocarbon group.

18. The dihydroxy compound according to claim 17, wherein in the formula (12), Z is a divalent hydrocarbon group having 1 to 6 carbon atoms.

19. In the formula (12), R 3 , R 4 and each independently represent a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. The dihydroxy compound according to any one of claims 16 to 18.

20. The dihydroxy compound according to any one of claims 16 to 19, wherein the formula (12) is the following formula (13) or the following formula (14): 【Chemistry 11】 【Chemistry 12】

Citation Information

Patent Citations

  • Tategatatendojikukesochi

    JP1976019250A

  • Low temperature welding

    JP1978046449A

  • Copolycarbonate polymer for binder of electrophotographic photoreceptor and its production

    JP1996311191A

  • Polycarbonate resin composition, and molded article, film, plate and injection-molded article each using the same

    JP2012214666A

  • JP2013、62