How to make cobalt sulfate
A method for producing highly pure cobalt sulfate from cobalt chloride solutions by sequential solvent extraction and crystallization effectively removes impurities, addressing inefficiencies and costs in existing methods.
Patent Information
- Application Number
- JP2021068292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-13
- Filing Date
- 2021-04-14
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-04-14
AI Technical Summary
Existing methods for producing cobalt sulfate are inefficient and costly, requiring multiple steps and electrolytic processes, and do not effectively remove impurities such as copper, zinc, manganese, calcium, and magnesium from cobalt chloride solutions, especially for applications in lithium-ion secondary batteries.
A method involving a copper removal step using a sulfiding agent to form copper sulfide precipitate, followed by solvent extraction steps with alkyl phosphate and carboxylic acid extractants to separate and remove impurities, and a crystallization step to obtain cobalt sulfate crystals, without using an electrolytic process.
This method allows for the direct production of highly pure cobalt sulfate by effectively removing impurities, reducing environmental impact, and lowering production costs by eliminating the need for electrolytic processes.
Smart Images

Figure 0007552487000008 
Figure 0007552487000009 
Figure 0007552487000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing cobalt sulfate, and more particularly to a method for producing high-purity cobalt sulfate by removing impurity elements contained in a cobalt chloride solution. [Background technology]
[0002] Cobalt is a valuable metal that is widely used in industrial applications as a raw material for magnetic materials and lithium-ion secondary batteries, in addition to its use as an additive element in special alloys. In particular, lithium-ion secondary batteries have recently come to be widely used as batteries for mobile devices and electric vehicles, and the demand for cobalt has been expanding rapidly accordingly. However, most cobalt is produced as a by-product of nickel and copper smelting, so separation of impurities, including nickel and copper, is an important elemental technology in the production of cobalt.
[0003] For example, when recovering cobalt as a by-product in the hydrometallurgy of nickel, the raw material is first leached or extracted into a solution or subjected to a dissolution treatment using a mineral acid, an oxidizing agent, etc., to obtain a solution containing nickel and cobalt. Furthermore, the nickel and cobalt contained in the obtained acidic solution are often separated and recovered by a solvent extraction method using various organic extractants according to a conventionally known method. However, the resulting cobalt solution often still contains various impurities derived from the raw materials used in the process.
[0004] Therefore, after nickel has been separated and recovered by the above-mentioned solvent extraction method, it is necessary to further remove impurity elements such as manganese, copper, zinc, calcium and magnesium from the cobalt solution. Furthermore, in order to produce a high-purity cobalt product with a low impurity content, it was necessary to remove impurity elements from a cobalt solution that had been separated and recovered from a nickel solution containing cobalt in advance, and then to commercialize the cobalt through an electrolysis process, crystallization, or the like.
[0005] Patent Documents 1 and 2 disclose conventional methods for removing impurity elements from a cobalt solution. Patent Document 1 discloses a method for purifying a cobalt solution, including: (1) a decopperizing step of adding a sulfiding agent to a cobalt solution and adjusting the oxidation-reduction potential (ORP) (based on Ag / AgCl electrode) to 50 mV or less and the pH to 0.3 to 2.4 to obtain a copper sulfide precipitate and a decopperized purified liquid; (2) a demanganizing step of adding an oxidizing agent and a neutralizing agent to the decopperized purified liquid and adjusting the oxidation-reduction potential (based on Ag / AgCl electrode) to 950 to 1050 mV and the pH to 2.4 to 3.0 to obtain a manganese precipitate and a demanganized purified liquid; and (3) a solvent extraction step of extracting and separating zinc, calcium and trace impurities in the demanganized purified liquid using alkyl phosphoric acid as an extractant. Patent Document 2 describes a technique in which a cobalt chloride solution having a hydrochloric acid concentration of 2 to 6 mol / L is brought into contact with an anion exchange resin to adsorb and separate metal impurities such as iron, zinc, and tin, which form complexes with a distribution coefficient for the anion exchange resin that is larger than that of a cobalt chloride complex.
[0006] The solvent extraction method using alkyl phosphoric acid as an extractant described in the above Patent Document 1 has high separation performance for zinc and calcium. However, in the case of a cobalt chloride solution with a hydrochloric acid concentration of 2 to 6 mol / L, an ion exchange method using an anion exchange resin and a solvent extraction method using an amine-based extractant have higher separation performance for zinc and cobalt than the above solvent extraction method using alkyl phosphoric acid. Furthermore, when removing very small amounts of zinc from a cobalt chloride solution, the ion exchange method is more efficient and economical because the process and operation are simpler.
[0007] From this perspective, a method has been proposed in which the purification method of Patent Document 1 and the separation technique of Patent Document 2 are combined to remove these impurity elements from a cobalt chloride solution containing manganese, copper, and zinc (e.g., Patent Document 3). The method for producing high-purity cobalt chloride described in paragraph 0022 of Patent Document 3 includes a solvent extraction step for separating nickel and cobalt, a demanganese step for removing manganese, a decopper step for removing copper, a dezincification step for removing zinc, and an electrolysis step. In the dezincification process, the aqueous cobalt chloride solution obtained in the decopperization process is brought into contact with an anion exchange resin to adsorb and remove zinc. In the electrolysis process, the high-purity aqueous cobalt chloride solution obtained in the dezincification process is used as an electrolytic feed solution to produce metallic cobalt (also known as electrolytic cobalt).
[0008] On the other hand, as mentioned above, the demand for cobalt as a raw material for lithium ion secondary batteries has recently increased, and the form of a cobalt sulfate solution or cobalt sulfate crystals is desired. To obtain cobalt sulfate crystals from metallic cobalt obtained by the conventional technique of Patent Document 3, metallic cobalt is dissolved in sulfuric acid to obtain a cobalt sulfate solution, and this solution is then crystallized to obtain cobalt sulfate crystals. However, this manufacturing method increases the manufacturing cost due to an increase in the number of steps and chemical costs. In addition, plate-shaped metallic cobalt, which is used in corrosion-resistant alloys, dissolves slowly in sulfuric acid, and in order to dissolve it in a short time, it is necessary to powder the plate-shaped metallic cobalt by atomization or the like. For this reason, a method for obtaining a cobalt sulfate solution directly from a cobalt chloride solution without going through metallic cobalt has been desired. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2004-285368 A [Patent Document 2] JP 2001-020021 A [Patent Document 3] JP 2020-19664 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been proposed in view of the above-mentioned circumstances, and has an object to provide a method for producing high-purity cobalt sulfate by separating impurities and cobalt from a cobalt chloride solution containing impurities without using an electrolysis process. [Means for solving the problem]
[0011] The method for producing cobalt sulfate of the first invention is to produce a cobalt sulfate containing copper, zinc, manganese, calcium and magnesium. home The process includes a copper removal step in which a sulfurizing agent is added to a cobalt chloride solution containing one or more types of impurities to generate a copper sulfide precipitate and separate and remove it, a first solvent extraction step in which an organic solvent containing an alkyl phosphoric acid extractant is contacted with the cobalt chloride solution that has been subjected to the copper removal step, and zinc, manganese, and calcium are extracted into the organic solvent and separated and removed, and a second solvent extraction step in which an organic solvent containing a carboxylic acid extractant is contacted with the cobalt chloride solution that has been subjected to the first solvent extraction step, and cobalt is extracted into the organic solvent, and then the cobalt is stripped with sulfuric acid to obtain a cobalt sulfate solution. The second solvent extraction step includes a solvent recovery process in which the cobalt chloride solution after cobalt extraction is contacted with the organic solvent after cobalt is stripped into a sulfuric acid solution to adjust the pH to 2.0 to 4.0, and the carboxylic acid extractant in the cobalt chloride solution is separated. It is characterized by: The method for producing cobalt sulfate according to the second invention is the same as that according to the first invention, except that in the copper removal step, a sulfurizing agent is added to cobalt chloride. to Add an oxidizing agent and a neutralizing agent to the solution to adjust the redox potential to -100 to 200 mV (based on an Ag / AgCl electrode) and the pH to 1.3 to 3.0. It is characterized by: The method for producing cobalt sulfate according to the third aspect of the present invention is characterized in that, in the first or second aspect of the present invention, the cobalt sulfate solution obtained through the second solvent extraction step is subjected to a crystallization step to obtain cobalt sulfate crystals. The fourth invention is a method for producing cobalt sulfate according to the first, second or third invention, characterized in that in the first solvent extraction step, the alkyl phosphate extractant is bis(2-ethylhexyl) hydrogen phosphate, and the pH of the cobalt chloride solution from which copper has been removed is adjusted to 1.5 to 3.0 and subjected to solvent extraction using the extractant, thereby extracting impurity elements into an organic solvent. The fifth invention is a method for producing cobalt sulfate according to the first, second or third invention, characterized in that in the second solvent extraction step, an alkaline solution is added to the cobalt chloride solution from which copper, zinc, manganese and calcium have been removed, to adjust the pH to 5.0 to 7.0, and a cobalt extraction step is carried out in which cobalt is extracted into an organic solvent using a carboxylic acid extractant. A sixth aspect of the present invention is a method for producing cobalt sulfate according to the fifth aspect of the present invention, characterized in that, following the cobalt extraction step in the second solvent extraction step, a cobalt stripping step is carried out in which the organic solvent in which cobalt has been extracted is contacted with a sulfuric acid solution to adjust the pH to 2.0 to 4.5, and cobalt is stripped into the sulfuric acid solution. 。 Effect of the Invention
[0012] According to the first invention, a high-purity cobalt sulfate solution from which impurities have been removed can be obtained by a decopperization process in which copper is precipitated as sulfide, a first solvent extraction process in which zinc, manganese and calcium are separated and removed, and a second solvent extraction process in which magnesium is separated and removed from a cobalt chloride solution containing impurities. Therefore, it is possible to directly produce high purity cobalt sulfate by separating impurities from cobalt without using an electrolysis process. In addition, by carrying out a solvent recovery process to separate the carboxylic acid extractant in the cobalt chloride solution in the second solvent extraction process, it is possible to prevent the organic solvent contained in the cobalt chloride solution after extraction from becoming a loss or increasing the environmental load due to wastewater. According to the second invention, copper sulfide can be precipitated and sufficiently removed from the cobalt chloride solution, and coprecipitation of cobalt can be suppressed. According to the third invention, by further carrying out a crystallization step, it is possible to obtain high-purity cobalt sulfate crystals from the cobalt sulfate solution. According to the fourth invention, bis(2-ethylhexyl) hydrogen phosphate is used as an alkyl phosphate extractant, which makes it easier to separate zinc, manganese, and calcium, which are impurities, from the cobalt solution. In addition, by adjusting the pH to 1.5 to 3.0, zinc, manganese, and calcium can be extracted and separated from cobalt, leaving cobalt in the aqueous phase. According to the fifth invention, by adjusting the pH to 5.0 to 7.0, cobalt can be extracted into the organic phase by contacting with an organic solvent containing a carboxylic acid extractant. According to the sixth invention, the cobalt extracted into the organic phase is brought into contact with a sulfuric acid solution, the pH is adjusted to 2.0 to 4.5, and the cobalt is stripped into the sulfuric acid solution, so that a high-purity cobalt sulfate solution can be obtained. 。 [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a process diagram showing a method for producing cobalt sulfate according to the present invention. [Diagram 2] FIG. 1 is a process diagram showing a method for producing cobalt sulfate according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a detailed process diagram of the first solvent extraction step S2 shown in FIG. 2. [Figure 4] FIG. 3 is a detailed process diagram of the second solvent extraction step S3 shown in FIG. 2. [Diagram 5] FIG. 13 is a detailed diagram of the solvent recovery process S32. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, specific embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications are possible without departing from the gist of the present invention.
[0015] (Basic principle of the present invention) The method for producing cobalt sulfate according to the present invention will be described with reference to FIG. This manufacturing method is characterized by carrying out the following steps in order. (1) A copper removal process S1 in which a sulfiding agent is added to a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium, and magnesium to generate a precipitate of copper sulfide and separate and remove it; (2) a first solvent extraction step S2 in which the cobalt chloride solution from which copper has been removed by the copper removal step S1 is contacted with an organic solvent containing an alkylphosphoric acid extractant to extract zinc, manganese and calcium into the organic solvent for separation and removal; (3) A second solvent extraction step S3 is carried out in which the cobalt chloride solution from which copper, zinc, manganese and calcium have been removed by the first solvent extraction step S2 is contacted with an organic solvent containing a carboxylic acid to extract cobalt into the organic solvent, and then the cobalt is stripped with sulfuric acid to obtain a cobalt sulfate solution. The second solvent extraction step S3 includes a solvent recovery treatment S32.
[0016] In the present invention, after each of the steps S1 to S3, a crystallization step S4 of precipitating crystals from the cobalt sulfate solution is carried out as necessary. Although not shown in FIG. 1, after the first solvent extraction step S2 and / or after the second solvent extraction step S3, a step of subjecting the liquid to an oil-water separation device such as an activated carbon column may be added to separate and remove organic components that have become mixed in the liquid.
[0017] The cobalt chloride solution used as the starting material in the present invention contains one or more of copper, zinc, manganese, calcium, and magnesium as impurity elements. The application of the present invention is not limited to any cobalt chloride solution containing such impurities, but it is particularly suitable for use in a cobalt chloride solution obtained after nickel is separated and recovered from a cobalt-containing nickel solution using an alkyl phosphoric acid extractant or an amine extractant in the solvent extraction process of nickel smelting.
[0018] According to the present invention, as shown in Fig. 2, a high-purity cobalt sulfate solution can be obtained by removing copper from a cobalt chloride solution by generating a copper sulfide precipitate in a copper removal step S1, separating and removing zinc, manganese and calcium in a first solvent extraction step S2, and separating and removing magnesium in a second solvent extraction step S3. Therefore, a high-purity cobalt sulfate solution can be produced directly by separating impurities and cobalt without using an electrolysis step. Then, the carboxylic acid extractant can be separated and recovered by a solvent recovery treatment S32 included in the second solvent extraction step S3.
[0019] Furthermore, according to the present invention, the cobalt sulfate solution that has been subjected to the steps S1 to S3 can be subjected to the crystallization step S4 to precipitate crystals from the solution, thereby obtaining cobalt sulfate crystals.
[0020] (Embodiment) Hereinafter, an embodiment of the method for producing cobalt sulfate will be described with reference to Fig. 2 to Fig. 5. Fig. 2 shows the details of steps S1 to S3 shown in Fig. 1.
[0021] (Copper removal process S1) The copper removal step S1 will be described with reference to FIG. The copper removal step S1 is carried out by adding a sulfurizing agent to the starting material, a cobalt chloride solution containing one or more impurities of copper, zinc, manganese, calcium, and magnesium. The amount of the sulfurizing agent added is adjusted, and a neutralizing agent is added as necessary to adjust the redox potential of the cobalt chloride solution to -100 to 200 mV (Ag / AgCl electrode standard) and the pH to 1.3 to 3.0. In step S1, a precipitate of copper sulfide is generated and separated from the cobalt chloride solution, thereby obtaining a cobalt chloride solution from which copper has been removed.
[0022] Copper in the cobalt chloride solution is removed from the solution by forming a copper sulfide precipitate according to Equation 1, Equation 2, or Equation 3 below. CuCl2+H2S→CuS↓+2HCl...(Formula 1) CuCl2+Na2S→CuS↓+2NaCl···(Formula 2) CuCl2+NaHS→CuS↓+NaCl+HCl···(Formula 3)
[0023] In the copper removal step S1, by adjusting the redox potential of the cobalt chloride solution to −100 to 200 mV (based on an Ag / AgCl electrode) and the pH to 1.3 to 3.0, copper can be sufficiently removed as sulfide and coprecipitation of cobalt can be suppressed. If the redox potential exceeds 200 mV, the copper in the solution is not sufficiently removed, and if it is less than -100 mV, the amount of cobalt co-precipitated increases, which is not preferable. If the pH is less than 1.3, the copper in the solution is not sufficiently removed and the filterability of the resulting sulfide precipitate deteriorates. If the pH exceeds 3.0, the amount of cobalt co-precipitated increases with the removal of copper, which is not preferable.
[0024] The oxidation-reduction potential can be adjusted by adjusting the amount of sulfurizing agent added. When the oxidation-reduction potential becomes lower than the desired value due to the addition of the sulfurizing agent, it can be adjusted by adding an oxidizing agent. For example, the oxidation-reduction potential can be adjusted by introducing air into the solution and stirring it, or by adding a hydrogen peroxide solution. The sulfurizing agent is not particularly limited, but hydrogen sulfide gas, sodium sulfide or sodium hydrosulfide crystals or aqueous solutions, etc., can be used. When hydrogen sulfide or sodium hydrosulfide is used as the sulfiding agent, the pH is adjusted by adjusting the amount of the sulfiding agent and adding a neutralizing agent. The neutralizing agent is not particularly limited, and alkali salts such as sodium hydroxide, calcium hydroxide, sodium carbonate, and cobalt carbonate can be used.
[0025] (First solvent extraction step S2) The first solvent extraction step S2 will be described with reference to FIGS. The first solvent extraction step S2 is a step in which the cobalt chloride solution that has been subjected to the copper removal step is contacted with an organic solvent containing an alkyl phosphoric acid-based extractant, and zinc, manganese and calcium are extracted into the organic solvent and separated and removed.
[0026] As the organic solvent, an alkyl phosphate extractant diluted with a diluent is used. Examples of alkyl phosphate extractants include bis(2-ethylhexyl) hydrogen phosphate (trade name D2EHPA), 2-ethylhexyl (2-ethylhexyl) phosphonic acid (trade name PC-88A), and di(2,4,4-trimethylpentyl) phosphinic acid (trade name CYANEX272). Among these, when separating zinc, manganese, and calcium from a cobalt chloride solution from which copper has been removed, it is preferable to use bis(2-ethylhexyl) hydrogen phosphate, which has high separability from cobalt, as an alkyl phosphate extractant. This is because bis(2-ethylhexyl) hydrogen phosphate has good properties for separating zinc, manganese, and calcium, which are impurities, from a cobalt solution.
[0027] The diluent is not particularly limited as long as it can dissolve the extractant. For example, naphthenic solvents and aromatic solvents can be used as the diluent. The concentration of the extractant is preferably adjusted to 10 to 60% by volume, more preferably 20 to 50% by volume. When the concentration of the extractant is within this range, impurity elements with high concentrations and impurity elements with low distribution ratios (element concentration in organic solvent / element concentration in solution) can be sufficiently extracted. On the other hand, when the concentration of the extractant is less than 10%, impurity elements with high concentrations and impurity elements with low distribution ratios cannot be sufficiently extracted, and tend to remain in the cobalt chloride solution. In addition, when the concentration of the extractant exceeds 60%, the viscosity of the organic solvent increases, and the phase separation property after the extraction operation of the organic solvent (organic phase) and the cobalt chloride solution (aqueous phase) deteriorates.
[0028] Acidic extractants such as alkyl phosphate extractants extract metal ions by forming metal salts by replacing the -H of the extractant with cations in the aqueous phase, as shown in formula 4. Generally, as the pH increases, metal ions are more easily extracted into the organic phase, and as the pH decreases, the reaction in formula 4 proceeds in the opposite direction, making it easier for metal ions extracted into the organic phase to be back-extracted into the aqueous phase. Since the pH at which metal ions are extracted varies depending on the type of metal ion, the pH is controlled in the solvent extraction process using an acidic extractant to separate the target element from impurity elements. nRH org + M n+ aq → MR norg + nH + aq ...(Formula 4) where RH is the acid extractant, M n+ indicates an n-valent metal ion, org indicates the organic phase, and aq indicates the aqueous phase.
[0029] Therefore, in the first solvent extraction step S2, it is desirable to adjust the pH of the cobalt chloride solution from which copper has been removed to 1.5 to 3.0. In this pH range, the extraction rates of zinc, manganese, and calcium tend to be higher than that of cobalt, and it is possible to separate these impurity elements from cobalt by extracting them into the organic phase while leaving cobalt in the aqueous phase.
[0030] If the pH is less than 1.5, the extraction rate of these impurities is low and separation from cobalt becomes difficult, and if the pH exceeds 3.0, the extraction rate of cobalt also increases and separation from impurities decreases. If the pH is adjusted to 1.5 to 3.0, some of the cobalt may be extracted, but it is also possible to reduce the loss of cobalt by contacting the organic phase after extraction with a hydrochloric acid solution with a lower pH than that used during extraction to recover the cobalt by back-extraction. Furthermore, when this organic phase is brought into contact with an acidic solution of pH 1 or less, most of the extracted metal ions can be back-extracted into the aqueous phase, allowing the organic phase after back-extraction to be reused.
[0031] (Second solvent extraction step S3) The second solvent extraction step S3 will be described with reference to Figs. 2, 4 and 5. The second solvent extraction step S3 is a step in which a cobalt extraction step S31 is carried out in which the cobalt chloride solution that has been subjected to the first solvent extraction step S2 is brought into contact with an organic solvent containing a carboxylic acid extractant to extract cobalt, and then a solvent recovery treatment S32 in which the carboxylic acid extractant is separated and recovered from the cobalt chloride solution after the cobalt has been extracted, and a cobalt stripping step S33 in which cobalt is stripped with sulfuric acid are carried out in parallel to obtain a cobalt sulfate solution.
[0032] The organic solvent used is a carboxylic acid extractant diluted with a diluent. Examples of carboxylic acid extractants include versatic acid and naphthenic acid. These are acidic extractants that contain COOH groups.
[0033] When extracting metal ions, carboxylic acid extractants release protons into the aqueous phase according to the valence of the metal, and the metal ion coordinates to the carbonyl oxygen. Many carboxylic acids form dimers and trimers through hydrogen bonds with each other in non-polar solvents. In addition, when extracting metal ions, carboxylic acids that have not been acid-dissociated may coordinate to remove the water of hydration coordinated to the metal ion. For example, in the case of a 6-coordinate divalent metal ion M 2+ The reaction in which is extracted by the dimeric carboxylic acid extractant R2H2 is represented as shown in Equation 5. [M(H2O)6] 2+ aq +3(R2H2) org → (MR2 4RH) org +2H + aq +6H2O aq ...(Formula 5) In the formula, org represents an organic phase and aq represents an aqueous phase.
[0034] (Cobalt extraction process S31) In the cobalt extraction step S31, an alkaline solution is added as a neutralizing agent to the cobalt chloride solution from which copper, zinc, manganese, and calcium have been removed, to adjust the pH to 5.0 to 7.0. When the pH is within this range, the cobalt can be extracted into the organic phase by contacting the solution with an organic solvent containing a carboxylic acid-based extractant. At this time, magnesium is not extracted and remains in the aqueous phase. If the pH is less than 5, it is difficult to extract cobalt, while if the pH exceeds 7, the solubility of cobalt decreases and precipitation may occur.
[0035] Specifically, a solution of sodium hydroxide or potassium hydroxide can be used as the alkaline solution. In order to prevent oxidation during extraction, bubbling with an inert gas such as nitrogen gas, argon gas, or carbon dioxide gas may be performed.
[0036] (Solvent recovery process S32 and cobalt stripping process S33) As shown in FIG. 2, after the cobalt extraction step S31, a solvent recovery process S32 and a cobalt stripping step S33 are carried out in parallel.
[0037] (Solvent recovery process S32) In the cobalt chloride solution (aqueous phase) obtained after the cobalt extraction step S31, some of the carboxylic acid extractant may be dissolved. This is not desirable because it results in a loss of the extractant and also has an impact on the environment due to TOC (total organic carbon) caused by the extractant when the aqueous phase is subjected to wastewater treatment and discharged into the sea, etc. To prevent this, it is advisable to carry out the solvent recovery process S32 shown in FIG. 4.
[0038] As shown in Fig. 5, the solvent recovery process S32 is a process in which the cobalt chloride solution (residual liquid) after cobalt extraction is brought into contact with one or more of the organic solvent after stripping, the carboxylic acid extractant, and the diluent, and a neutralizing agent or acid is added to adjust the pH to 2.0 to 4.0, and the carboxylic acid extractant in the cobalt chloride solution is separated and recovered. This solvent recovery process S32 can prevent the loss of organic solvent and can also suppress the environmental load of wastewater (an increase in TOC concentration due to dissolution of the carboxylic acid extractant in the aqueous phase).
[0039] (Cobalt back extraction process S33) As shown in Fig. 4, in the cobalt stripping step S33, the cobalt extracted with the carboxylic acid extractant obtained in the cobalt extraction step S31 is brought into contact with a sulfuric acid solution to adjust the pH to 2.0 to 4.5. This allows the cobalt to be stripped into the sulfuric acid solution. In this way, a high-purity cobalt sulfate solution is obtained. Although back extraction is possible even at a pH of less than 2, lowering the pH too much does not change the recovery amount much and the effect is small. On the other hand, it is not preferable because the amount of back extraction of trace impurities extracted at a pH lower than cobalt increases. In addition, there are issues such as the cost of chemicals, so it is better to set the pH at 2.0 or higher. On the other hand, it is not preferable to set the pH above 4.5 because the back extraction rate of cobalt decreases and the recovery amount of cobalt decreases.
[0040] Since the organic phase obtained after extraction in the cobalt extraction step S31 still contains fine aqueous phase particles even after phase separation, a washing step may be added to remove the aqueous phase before stripping. For the aqueous phase in the washing step, a cobalt sulfate solution may be used, for example. In addition, the organic phase obtained after stripping in the cobalt stripping step S33 can be reused as the organic phase used in the solvent recovery process S32.
[0041] By the above method, a high-purity cobalt sulfate solution with few impurities can be produced.
[0042] (Crystallization step S4) The crystallization step S4 will be described with reference to FIG. In the crystallization step S4, crystals of cobalt sulfate are precipitated from the cobalt sulfate solution obtained in the second solvent extraction step S3. The crystallization method is not particularly limited, and can be performed using a general crystallization method.
[0043] For example, a method of obtaining crystals by placing a cobalt sulfate solution in a crystallizer and crystallizing in the crystallizer can be mentioned. The crystallizer is a device for precipitating crystals by evaporating water in the cobalt sulfate solution under a predetermined pressure, and for example, a rotary evaporator or a double propeller type crystallizer is used. The internal pressure is reduced by a vacuum pump or the like, and in the rotary evaporator, crystallization proceeds while rotating the flask and stirring with a double propeller. In the crystallizer, the cobalt sulfate solution is mixed with cobalt sulfate crystals to form a slurry.
[0044] The slurry discharged from the crystallizer is separated into cobalt sulfate crystals and mother liquor by a filter, a centrifuge, etc. The cobalt sulfate crystals are then dried in a dryer to remove moisture. By the above method, cobalt sulfate crystals can be produced from the cobalt sulfate solution. Of course, since the cobalt sulfate solution is highly pure with few impurities, the obtained cobalt sulfate crystals are also highly pure with few impurities. EXAMPLES
[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0046] [Example 1] (Copper removal process S1) A sodium hydrosulfide solution was added as a sulfiding agent to 2 L of a cobalt chloride solution having the composition shown in original solution A in Table 1, which had been adjusted to pH 2.5, and the oxidation-reduction potential was adjusted to -50 mV (Ag / AgCl electrode standard) to generate a precipitate of copper sulfide. The precipitate was separated and removed using a filter, and a filtrate having the composition shown in post-sulfidation B in Table 1 was obtained. The copper concentration was less than 0.001 g / L, and copper was successfully separated and removed.
[0047] (First solvent extraction step S2) An organic phase was prepared by diluting an alkyl phosphoric acid extractant (trade name D2EHPA, manufactured by Daihachi Chemical Industry Co., Ltd.) with a diluent (trade name Teclean N20, manufactured by JX Nippon Oil & Energy Corporation) so that the concentration was 40% by volume. 0.9 L of the aqueous phase consisting of the cobalt chloride solution obtained in the copper removal step S1 and 1.8 L of the organic phase were mixed, and a sodium hydroxide solution was added to adjust the pH to 1.7, and impurities were extracted. The same extraction operation was repeated with 0.9 L of the aqueous phase after extraction and 1.8 L of new organic phase, for a total of three extraction operations. As a result, a cobalt chloride solution with the composition shown in Table 1, 1SX after C was obtained. The concentrations of zinc, manganese, and calcium were all less than 0.001 g / L, and these impurities were able to be separated and removed.
[0048] (Second solvent extraction step S3) An organic phase was prepared by diluting a carboxylic acid extractant (product name: Versatic Acid 10, manufactured by Oxalis Chemicals) with a diluent (Teclean N20) so that the concentration was 30% by volume. 0.44 L of the aqueous phase consisting of the cobalt chloride solution obtained in the first solvent extraction step S2 was mixed with 1 L of the organic phase, and sodium hydroxide solution was added to adjust the pH to 6.5, and cobalt was extracted into the organic phase (cobalt extraction step S31). 0.6L of the extracted organic phase was mixed with 0.6L of a cobalt chloride solution with a cobalt concentration of 10g / L, and the aqueous phase that had been mixed into the organic phase after extraction was washed. Subsequently, this organic phase was mixed with 0.09L of pure water, and sulfuric acid was added to adjust the pH to 4, and cobalt was stripped (cobalt stripping step S33). As a result, a cobalt sulfate solution with the composition shown in Table 1, 2SX after D was obtained. The magnesium concentration was less than 0.001g / L, and magnesium was successfully separated and removed. By the above method, a high purity cobalt sulfate solution was obtained.
[0049] [Table 1]
[0050] (Crystallization step S4) The cobalt sulfate solution was placed in a rotary evaporator, and the inside of the rotary evaporator was decompressed with a vacuum pump while the temperature was maintained at 40°C. The water was evaporated while rotating the flask, and cobalt sulfate crystals were precipitated. After solid-liquid separation, the obtained cobalt sulfate crystals were dried in a dryer. As a result, high-purity cobalt sulfate crystals as shown in Table 2 were obtained. [Table 2]
[0051] [Example 2] A cobalt sulfate solution was obtained in the same manner as in Example 1, except that in the copper removal step S1, the oxidation-reduction potential was adjusted to 150 mV (Ag / AgCl electrode standard), in the second solvent extraction step S3, 0.44 L of an aqueous phase obtained by diluting the cobalt chloride solution obtained in the first solvent extraction step S2 by two times with pure water was mixed with the organic phase (cobalt extraction step S31), 0.6 L of the extracted organic phase was mixed with 0.6 L of a cobalt chloride solution having a cobalt concentration of 10 g / L to wash the aqueous phase that had been mixed in the organic phase after extraction, and this organic phase was mixed with 0.08 L of pure water, and sulfuric acid was added to adjust the pH to 4 to strip-extract cobalt (cobalt strip-extraction step S33). The composition in this case is shown in Table 3. As shown in Table 3, after 2SX, D, a high purity cobalt sulfate solution was obtained. [Table 3]
[0052] Subsequently, crystallization was carried out in the same manner as in Example 1, and high-purity cobalt sulfate crystals as shown in Table 4 were obtained. [Table 4]
[0053] [Example 3] A cobalt sulfate solution was obtained in the same manner as in Example 1, except that the solvent recovery process S32 was carried out. In the solvent recovery process S32, sulfuric acid was added to the cobalt chloride solution showing a pH of 6.5 after the cobalt was extracted in the cobalt extraction step S31, and the pH was adjusted to 2 to 4 to separate and recover the carboxylic acid extractant. Then, the TOC concentration in the cobalt chloride solution was measured using a known method. As shown in Table 5, by reducing the pH to 4 or less, the TOC content of 260 mg / l was reduced to a level of 100 mg / l, that is, the carboxylic acid extractant was separated from the cobalt chloride solution. As a result, it was possible to suppress the loss of the extractant, and to reduce the environmental load when the cobalt chloride solution after extraction was treated for wastewater and discharged into the sea, etc. [Table 5]
[0054] From the results of Examples 1, 2 and 3 above, it is clear that according to the present invention, it is possible to obtain cobalt sulfate with high purity from which impurities have been sufficiently removed. [Industrial Applicability]
[0055] The highly pure cobalt sulfate crystals obtained by the present invention can be used as a raw material for lithium ion secondary batteries and can also be used for a variety of other purposes. [Explanation of symbols]
[0056] S1 Copper removal process S2 1st solvent extraction step S3 Second solvent extraction process S4 Crystallization process S31 Cobalt Extraction Process S32 Solvent recovery treatment S33 Cobalt stripping process
Claims
1. A copper removal process in which a sulfiding agent is added to a cobalt chloride solution containing one or more impurities selected from the group consisting of copper, zinc, manganese, calcium, and magnesium, to generate copper sulfide precipitates, which are then separated and removed; a first solvent extraction step in which an organic solvent containing an alkylphosphoric acid extractant is contacted with the cobalt chloride solution that has been subjected to the copper removal step, and zinc, manganese and calcium are extracted into the organic solvent to be separated and removed; a second solvent extraction step in which the cobalt chloride solution obtained in the first solvent extraction step is contacted with an organic solvent containing a carboxylic acid extractant to extract the cobalt into the organic solvent, and then the cobalt is stripped with sulfuric acid to obtain a cobalt sulfate solution; Execute the following in order. The second solvent extraction step includes a solvent recovery process in which the cobalt chloride solution after extraction of cobalt is contacted with the organic solvent after stripping cobalt into a sulfuric acid solution, the pH is adjusted to 2.0 to 4.0, and the carboxylic acid extractant in the cobalt chloride solution is separated. A method for producing cobalt sulfate comprising the steps of:
2. In the copper removal step, an oxidizing agent and a neutralizing agent are added to the cobalt chloride solution to which a sulfiding agent has been added, so as to adjust the redox potential to −100 to 200 mV (based on an Ag / AgCl electrode) and the pH to 1.3 to 3.
0.
2. The method for producing cobalt sulfate according to claim 1 .
3. The cobalt sulfate solution obtained through the second solvent extraction step is subjected to a crystallization step to obtain cobalt sulfate crystals.
3. The method for producing cobalt sulfate according to claim 1 or 2.
4. In the first solvent extraction step, the alkyl phosphate extractant is bis(2-ethylhexyl) hydrogen phosphate; The pH of the cobalt chloride solution from which copper has been removed is adjusted to 1.5 to 3.0, and the solution is subjected to solvent extraction using the extractant to extract impurity elements into an organic solvent. The method for producing cobalt sulfate according to claim 1, 2 or 3.
5. In the second solvent extraction step, an alkaline solution is added to the cobalt chloride solution from which copper, zinc, manganese and calcium have been removed to adjust the pH to 5.0 to 7.0, and a cobalt extraction step is carried out in which cobalt is extracted into an organic solvent using a carboxylic acid-based extractant. The method for producing cobalt sulfate according to claim 1, 2 or 3.
6. Following the cobalt extraction step in the second solvent extraction step, a cobalt stripping step is carried out in which the organic solvent from which the cobalt has been extracted is contacted with a sulfuric acid solution to adjust the pH to 2.0 to 4.5, and the cobalt is stripped into the sulfuric acid solution. The method for producing cobalt sulfate according to claim 5 .
Citation Information
Patent Citations
Production of high purity cobalt solution
JP2000017347A
Manufacture of high purity cobalt
JP2001020021A
Method for refining cobalt aqueous solution
JP2004285368A
Method for producing cobalt sulfate
JP2012153546A
Cobalt extractant and cobalt extraction method
JP2013129905A