Moisture-curable polyolefin formulations
A catalyst system using transition metal acetylacetonates and (aza)carboxamidines addresses the need for safer and more efficient curing of polyolefins, enhancing condensation reactions and improving the properties of cured polyolefin products.
Patent Information
- Application Number
- JP2023043681
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2039-02-13
AI Technical Summary
Existing moisture-curable polyolefin formulations often rely on toxic and environmentally harmful catalysts, and there is a need for a safer and more efficient curing system that enhances the condensation of polyolefins.
A catalyst system based on transition metal acetylacetonate compounds, specifically cobalt and zinc acetylacetonate, combined with (aza)carboxamidines, is used to enhance the condensation curing of polyolefins, providing a non-toxic and effective alternative.
The proposed catalyst system improves the curing process by enhancing condensation reactions while being environmentally safe and non-toxic, resulting in improved mechanical properties and processing characteristics of the cured polyolefin products.
Smart Images

Figure 0007554864000004 
Figure 0007554864000002 
Figure 0007554864000001
Abstract
Description
[Technical field]
[0001] Moisture-curable polyolefin formulations and related aspects.
[0002] Introduction Published patent applications and patents in or relating to this field are US2009 / 0156 737(A1), US2011 / 0046304(A1), US2011 / 009842 0(A1), US2014 / 0329090(A1), US2016 / 0319081( A1), US2018 / 0244828(A1), US4293597, US44618 67, US5945466, US5985991, US7365145, US74857 29(B2), US7527838(B2), US8877885(B2), US900 6357(B2), US9175188(B2), US9328205(B2), and Includes US9976028(B2). Summary of the Invention [Problem to be solved by the invention]
[0003] We have demonstrated that a curing catalyst system based on certain transition metal acetylacetonate compounds is effective in preventing moisture curing. The present invention enhances the condensation of photosensitive polyolefins and is therefore useful as an environmentally safe, non-toxic catalyst. Our technical solution is to use (hydrolyzable silyl group)-functional polyolefins. A fin prepolymer and a compound which is a carboxamidine or guanidine and a cobalt a and mixtures with compounds that are cetylacetonate or zinc acetylacetonate. and / or a condensation cure catalyst system made therefrom, each compound independently being a non-substituted The present invention also includes a moisture curable polyolefin formulation which is or has been substituted. and methods of use, cured polyolefins made therefrom, and compositions containing the same. Also included are condensation cured polymers useful therein or articles made therefrom. Also included are catalytic systems. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0004] The summary and abstract are incorporated herein by reference. , including the following numbered aspects and detailed description.
[0005] Aspect 1. A moisture-curable polyolefin formulation comprising: (A) a hydrolyzable silyl group; (B) a -functional polyolefin prepolymer, The compounds may be unsubstituted or substituted (collectively referred to as "(aza)carboxamidines"). ) with a cobalt acetylacetonate or zinc acetylacetonate coordination complex In compounds in which each acetylacetonate is independently unsubstituted ("aca or substituted with 1 to 5 alkyl groups (abbreviated as "alkyl-acac"). (abbreviated), compounds in which each alkyl group is unsubstituted ("Co,Zn(alkyl)acetylacetonate" By contacting the compound with Co,Zn(alkyl)acac, the compound is and a condensation cure catalyst system comprising a mixture made by ) acetylacetonate is a cobalt(II)((alkyl)acetylacetonate)2 (abbreviated as Co(II)((alkyl)acac)2), cobalt(III) ((alkyl) Co(III)((alkyl)acetylacetonate)3 (abbreviated as Co(III)((alkyl)acac)3) ), and zinc(II)((alkyl)acetylacetonate)2(Zn(II) ((alkyl)acac)2) In each of the mixtures, the amount of (A) is 79.0 to 99.99 weight percent (wt%). and the amount of (B) is 21.0 to 0.01% by weight, and the (B) condensation curing catalyst system is 1 5:0.15 (aza)carboxamidine / Co,Zn(alkyl)acetylacetoner The moisture curable polyolefin formulation is characterized by a molar ratio of , The guanidine may be a compound of formula (I) as described below. The guanidine may be a compound of formula (II) as described below. Co,Zn(alkyl)acetylacetonates are obtained by reacting Co(II)((alkyl)a cac)2 and Co(III)((alkyl)acac)3, or from Co(II )((alkyl)acac)2 and Zn(II)((alkyl)acac)2, or Co(III)((alkyl)acac)3 and Zn(II)((alkyl)a cac)2, or Co(II)((alkyl)acac)2, or Co (III)((alkyl)acac)3 or Zn(II)((alkyl)ac The moisture-curable polyolefin formulation may be selected from (A) and (B). Alternatively, the moisture-curable polyolefin formulation may comprise (A) and (B). and furthermore (A), (B), (aza)carboxamidine, or Co,Zn(alanine). may contain at least one additive that is not acetylacetonate, all of which are moisture resistant. Based on the total weight of the curable polyolefin formulation, the amount of (A) is 79.1 to 99.89 wt. The amount of (B) may be 0.01 to 20.8% by weight, and at least one additive The total amount of the additives may be 0.10 to 20.89% by weight. Examples are provided below.
[0006] Aspect 2. (A) A (hydrolyzable silyl group)-functional polyolefin prepolymer is Limitations (i) to (iii): (i) each hydrolyzable silyl group is independently represented by the formula (R 2 ) m (R 3 ) 3-m Si-(II), where the subscript m is an integer of 1, 2, or 3. number, each R 2 are independently H, HO-, (C1-C6)alkoxy, (C2-C6) Carboxy, phenoxy, (C1-C6) alkyl)-phenoxy, ((C1-C6) a (C1-C6)alkyl(H)C=NO-, or ((C1-C6)a R = NO-, 3 are independently (C1-C6) alkyl or phenyl (ii) the polyolefin portion of (A) is a polyethylene-based, poly(ethylene- Co-(C3-C 40 ) alpha-olefins) or combinations thereof. and (iii) both (i) and (ii). Moisture-curable polyolefin compound of each R 2 may not contain H and HO- , or may be free of phenoxy and (C1-C6) alkyl-phenoxy. Each R 2 are independently (C1-C6)alkoxy, (C2-C6)carboxy, ((C1 -C6) alkyl)2N-, (C1-C6) alkyl(H)C=NO-, or ((C1 -C6) alkyl) 2C=NO-; or (C1-C6) alkoxy; or (C2-C6) carboxy; or ((C1-C6) alkyl)2N-; or (C1-C6)alkyl(H)C=NO-; or ((C1-C6)alkyl)2C =NO- is possible.
[0007] Aspect 3. (B) The mixture of the condensation curing catalyst system is (B1) to (B3): (B1) (aza) ka Blends of ruboxamidine with Co,Zn(alkyl)acetylacetonates; (B2) Reaction of (aza)carboxamidine with Co,Zn(alkyl)acetylacetonates. (B3) (B2) reaction product and (aza) carboxylate in combination with samidine and / or Co,Zn(alkyl)acetylacetonates; 3. The moisture curable polyolefin formulation of embodiment 1 or 2, wherein
[0008] Aspect 4. (Alkyl)Co,Zn(alkyl)acetylacetonates ) acetylacetonate is independently an unsubstituted acetylacetonate or (C1-C6 ) alkyl-substituted acetylacetonates, or unsubstituted acetylacetonates (i.e. , 2,4-pentanedionate), or (C1-C6) alkyl-substituted acetylacetonate 2,4-pentanedionate (i.e., (C1-C6) alkyl substituted 2,4-pentanedionate); The moisture curable polyolefin formulation of any one of embodiments 1 to 3. The alkyl-substituted acetylacetonates are independently selected from 1 to 5 (C1-C6) alkyl groups, or 1 to 4 (C1-C6) alkyl groups, or 1 to 3 (C1-C6) alkyl groups group, or 2 to 5 (C1-C6) alkyl groups, or 2 to 4 (C1-C6) An alkyl group, or one (C1-C6) alkyl group, or two (C1-C6) alkyl groups, each (C1-C6) alkyl group being unsubstituted and independently selected. Unsubstituted acetylacetonates are enolates of the formula H3CC(=O)C(H)=C(O-)CH3. Alternatively, at least one (alkyl)acetylacetonate may be depicted as or all but one (alkyl) acetylacetonate, or each (alkyl) acetylacetonate The alkyl)acetylacetonates may independently be alkyl-substituted acetylacetonates. Any remaining (alkyl)acetylacetonates may be unsubstituted. Cetylacetonate has the formula R a 3CC(=O)C(R b )=C(O-)CR c Enola 3 It can be drawn as a a ~R c At least one of is unsubstituted (C1-C6) alkyl. and any remaining R a ~R c Each of is independently H or an unsubstituted (C1-C6) alkyl group. In some embodiments, up to two or R a ~R c Only one of is unsubstituted (C1-C6) alkyl, and any remaining R a ~R c Each of is H. In some embodiments, each R a and R c is H and R b is unsubstituted (C1-C6) alkyl In some embodiments, all R a and R b And two R c is H, 1 R c is unsubstituted (C1-C6) alkyl. In some embodiments, unsubstituted (C1- C6) alkyl is methyl. In some embodiments, each unsubstituted (C1-C6) alkyl are independently unsubstituted (C1-C3) alkyl or unsubstituted (C4-C6) alkyl or unsubstituted (C2-C5) alkyl, or methyl, or ethyl, or Unsubstituted (C3) alkyl group, or unsubstituted (C4) alkyl group, or unsubstituted (C5 ) alkyl group or unsubstituted (C6) alkyl group. Alkyl-substituted acetylacetonates An example of an acetylacetonate is 3-methyl-acetylacetonate (R b is methyl, and each R a and R c is H) and 1,1,5,5-tetramethyl-acetylacetonate (R b teeth H and two R a is methyl and two R c is methyl, and the remaining R a and R c is H. Each (alkyl)acetylacetonate is independently an unsubstituted acetoacetate. acetylacetonate or methyl-substituted acetylacetonate, or 3-methyl-acetylacetonate acetylacetonate or 1,1,5,5-tetramethyl-acetylacetonate substituted acetylacetonates or unsubstituted acetylacetonates.
[0009] 5. (Aza)carboxamidines are unsubstituted or substituted carboxamidines. The moisture curable polyolefin formulation of any of embodiments 1 to 4, wherein the polyolefin is a carboxylic acid amine. The gin is represented by the formula (I): R 2 R 3 NC(=NR 1 )-C(R 4 )3(I) obtained, in the formula, R 1 ~R 4is the limit (r1)~(r4):(r1)R 1 ~R 4 Each of the following is independent: Then, H or (C1-C 45 ) a hydrocarbyl group; (r2) R 1 ~R 4 Either or two are bonded together (C1-C 45 ) hydrocarbylene, and the remaining R 1 ~R 4 Each of is independently H or (C 45 ) a hydrocarbyl group; (r3) R 1 ~R 4 Any three of these are bonded together to form a trivalent (C1-C 45 ) Hydrocarbon triradical group Form the remaining R 1 ~R 4 is H or (C1-C 45 ) a hydrocarbyl group, and (r4)R 1 ~R 4 All of the bonds together form a tetravalent (C1-C 45 ) Hydrocarbon tetrachloride forming a dicarbamidine group. may not contain an NH group. In this case, the moisture curable polyolefin formulation may be free of guanidine.
[0010] Aspect 6. Carboxamidines are (i) to (xix): (i) 1,8-diazabicyclo[ 5.4.0]undec-7-ene ("DBU"), (ii) 1,5-diazabicyclo[4 .3.0]non-5-ene DBN, (iii) 1,2,4-triazole-1-carboxylate (iv) acetamidine, (v) aminoacetamidine, (vi) benzamide (vii) 4-amino-benzamidine, (viii) 4-bromo-benzamidine (ix) 4-chlorobenzamidine, (x) 4-fluorobenzamidine, (xi ) 4-hydroxybenzamidine, (xii) 4-methoxybenzamidine, (xii i) 4-methylbenzamidine, (xiv) 4-trifluoromethylbenzamidine, ( xv) N,N'-formamidine, (xvi) N,N'-diphenylformamidine, ( xvii) Pivalamidine (i.e., 2,2-dimethylpropaneamidine or 2,2- Dimethylpropaneimidamide, CAS 18202-73-8), (xviii) 3-Bis(dimethylamino) Lysine-3-carboxyimidamide, and (xix) cyclopropylamidine The moisture-curable polyolefin formulation of embodiment 5, wherein the carboxamidine is one of: ) DBU or (ii) DBN.
[0011] 7. The (aza)carboxamidine is an unsubstituted or substituted guanidine. The moisture-curable polyolefin formulation according to any one of the preceding embodiments, wherein the guanidinium salt is The compound of formula (II) R 6 R 7 NC(=NR 5 )-NR 8 R 9 (II) , where R 5 ~R 9 is the limit (r1)~(r5):(r1)R 5 ~R 9 Each of the following is independent: , H or (C1-C 45 ) a hydrocarbyl group; (r2) R 5 ~R 9 Either The two are bonded together (C1-C 45 ) hydrocarbylene, and the remaining R 5 ~R 9 of Each independently is H or (C 45 ) a hydrocarbyl group; (r3) R 5 ~ R 9 Any three of these are bonded together to form a trivalent (C1-C 45 ) Hydrocarbon triradical group Formation and remaining R 5 ~R 9 Each of is independently H or (C 45 ) Hydrocarbohydrates (r4) R 5 ~R 9 Any four of these are bonded together to form a tetravalent (C1-C 45 ) forms a hydrocarbon tetraradical group, R 5 ~R 9 The remaining one is H or (C1-C4 5) a hydrocarbyl group, and (r5) R 5 ~R 9 All of the bonds together form a pentavalent (C1-C 45 ) forming a hydrocarbon pentaradical group. Guanidine is an aza-nitrogen bonded to the carbon atom of the carboxamidino group. For example, the compound represented by the formula (II) Aza nitrogen atom is R 8 and R 9 The guanidine does not have to contain an NH group. When the (aza)carboxamidine is guanidine, it is mixed with moisture-curing polyolefin. The article may be free of carboxamidines.
[0012] Aspect 8. Guanidine is (i) to (viii): (i) 1,5,7-triazabicyclo [4.4.0] Deca-5-ene ("TBD"), 7-methyl-1,5,7-triazabicyclo[4.4.0] chloro[4.4.0]dec-5-ene, (iii) 1,1,3,3-tetramethylguanidinium ("TMG", CAS 80-70-6), (iv) 1,1,2,3,3-pentamethyl guanidine ("PMG"), (v) 2-tert-butyl-1,1,3,3-tetramethyl (vi) 1,8-bis(tetramethylguanidino)naphthalene ("tBTMG"); (vii) 1-aminopyrazole, and (viii) 1H-pyrazole-1 -carboxamide. The guanidine may include (iii) TMG, (iv) PMG, or (v) tBTMG. .
[0013] Aspect 9. Additives (C) to (L): (C) organic peroxide, (D) scorch retarder, (E ) antioxidants, (F) tree retarders (water tree and / or electrical tree retarders), (G ) colorant, (H) moisture scavenger, (I) hindered amine light stabilizer (HALS), (J) additive (K) moisture generating agent, and (L) a combination of two or more of (C) to (K). and further comprising at least one additive selected from among Moisture-curable polyolefin compound. (L) may be any two or any combination of There may be three, or each of (D), (E), (F), and (I).
[0014] Aspect 10. A method of making a moisture-curable polyolefin formulation comprising: (A) (a) hydrating (B) a decomposable silyl group-functional polyolefin prepolymer and (B) a condensation curing catalyst system. (A) mixing components containing (A) and (B) to obtain a mixture containing (A) and (B); and (B) melting the mixture. or extruding to produce the moisture curable polyolefin formulation of any one of embodiments 1-9. When (B) is made in situ, the method includes melting (A) and then melting (A). First, Co,Zn(alkyl)acetylacetonate was added to the melt, and then (aza ) Carboxamidine is added to (B) the in situ prepared moisture curable polyolefin blend. When (B) is prepared in advance, first prepare a mixture of (aza)carboxamidine and Co. Zn(alkyl)acetylacetonate were mixed together to prepare (B), and (A (B) is added to the melt of (A) to form a moisture-curable polyolefin. The moisture curable polyolefin compound thus prepared is then extruded. The moisture curable polyolefin formulation is extruded, pelletized, and / or molded into a solid form. The product can be obtained as a molded or pelletized form. (B), and at least one additive selected from additives (C) to (L). The components are mixed to obtain a mixture containing at least one of (A), (B), and (C) to (L). and melting or extruding the mixture to obtain (A), (B), and (C) to (L and making an embodiment of the formulation including at least one additive of the following: Instead of adding (C), add (A), (B), and any of (D) to (K). After the melting or extrusion step containing the compound, the additive (C) organic peroxide is immersed in the compound. Thus, a formulation further comprising the immersed (C) organic peroxide can be obtained.
[0015] Aspect 11. The moisture-curable polyolefin formulation of any one of aspects 1 to 9, or The moisture-curable polyolefin formulation prepared by the method of Example 10 is moisture-cured to obtain a moisture-curable polyolefin composition. Moisture cured polyolefin product produced by obtaining an air cured polyolefin product The moisture curable polyolefin formulation may be moisture cured in its solid or molten state. do.
[0016] Aspect 12. The moisture-curable polyolefin formulation of any one of aspects 1 to 9, or 11. An article of manufacture comprising a shaped form of the moisture cured polyolefin product of claim 11. Examples include substrates, There are films, layers of laminates, and coatings on pipes.
[0017] Aspect 13. A coated conductor, comprising: a conductive core; and a conductive core at least partially separated from the conductive core. and a polymer layer surrounding the polymer layer, wherein at least a portion of the polymer layer is the moisture-curable polymer of embodiment 11. The entire polymer layer is made of a moisture cured polyolefin product. The conductive core may be linear (e.g., wire-like) and may have a length and a linear shape. and a proximal end and a distal end spaced apart from each other by a length of The coated conductor may completely surround the conductive core except for the proximal and distal ends. One or more additional polymer layers (which may independently comprise a moisture cured polyolefin product) ), and / or an outer shielding layer (e.g., a metal sheath or The support may further include a support member (e.g., a support member or a sleeve).
[0018] A method of conducting electricity, comprising: applying electricity to the entire conductive core of the coated conductor of claim 13. applying pressure to generate electrical flow through the conductive core. may have a length and proximal and distal ends spaced apart by the length, and the electrical current is conducted through a conductive core can flow the length of the tubing from the proximal end to the distal end or vice versa.
[0019] Aspect 15. A condensation cure catalyst system comprising a 1.5:1 to 2.4:1 (e.g., 2.0:1 DBU with a molar ratio of DBU / Co(II)((alkyl)acac)2 of 0.0 and C o(II)((alkyl)acac)2, 1:1 to 2:1 (e.g., 1.0: DBU / Co(III)((alkyl)acac)3 in a ratio of 1.0 or 2.0:1.0 A mixture of DBU and Co(III)((alkyl)acac)3 with a molar ratio of 1.5 :1 to 2.4:1 (e.g., 2.3:1.0) of TMG / Zn(II)((alkyl)a Mixtures of TMG and Zn(II)((alkyl)acac)2 with a molar ratio of 2 0.19:1 to 10:1 (e.g., 0.19:1.0, 1.7:1.0, 5.0:1 0.0, or 10.0:1.0) of DBU / Zn(II)((alkyl)acac)2 moiety. Mixtures of DBU and Zn(II)((alkyl)acac)2 with a ratio of 1. DBN / Zn(II)((alkyl)acac) ratio of 5:1 to 2.4:1 (e.g., 2:1) From a mixture of DBN and Zn(II)((alkyl)acac)2 with a molar ratio of 2 DBN is selected from the group consisting of 1,5-diazabicyclo[4.3.0]non-5-ene. DBU is 1,8-diazabicyclo[5.4.0]undec-7-ene, and TM G is tetramethylguanidine, and each (alkyl)acac is independently 1 to 5 Unsubstituted acetylacetonates with unsubstituted (C1-C6) alkyl groups or (C1-C 6) A condensation cure catalyst system which is an alkyl substituted acetylacetonate. (A) (hydrolyzable silyl group)-functional polyolefin prepolymer in situ Alternatively, (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer may be prepared. The mixture may be preformed separately from the polymers and prior to being combined. Each (alkyl) of embodiment 15 may be a mixture of any one of the embodiments of the invention. acac is unsubstituted or methyl-substituted acetylacetonate; or 3-methyl-acetylacetonate or 1,1,5,5-tetramethyl-acetyl Acetonates, methyl-substituted acetylacetonates, or unsubstituted acetylacetonates The (B) condensation curing catalyst system of any one of the embodiments 1 to 14 may be the condensation curing catalyst system of the embodiment 15. It may be a combined curing catalyst system.
[0020] Moisture-curable polyolefin composition. All components in the moisture-curable polyolefin formulation The total weight of the components is 100.00% by weight. Moisture curable polyolefin formulations contain water. It may be free of water (anhydrous) or may further comprise water.
[0021] The moisture curable polyolefin composition may be a one-part formulation or a multi-part formulation, e.g. It may be a two-part formulation. A two-part formulation may include a first and a second part, the first part being The present invention relates to a method for producing a polyolefin prepolymer comprising the steps of: (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer; and (B) a condensation copolymer. The second part consists essentially of a synthetic curing catalyst system, and the second part consists essentially of an additional part of (A) and optionally It essentially consists of one or more of the components (C) to (L).
[0022] Moisture curable polyolefin formulations are available as continuous (monolithic) or divided solids. The moisture curable polyolefin formulation may be in the form of granules and / or pellets. Prior to the mixing step used to prepare the moisture curable polyolefin formulation. In addition, (A) the (hydrolyzable silyl group)-functional polyolefin prepolymer is also split. The pharmaceutical composition may be in a solid form (e.g., granules or pellets).
[0023] The moisture-curable polyolefin formulation comprises (A) a (hydrolyzable silyl group)-functional polyolefin. The olefin prepolymer is then mixed with a catalyst masterbatch containing (B) a dispersion of a condensation curing catalyst system in a carrier resin. - Combined with a batch, a moisture-curable polyolefin comprising (A), (B), and a carrier resin The (B) carrier resin may be prepared by adding an additional amount of (A), or polyethylene homopolymer, ethylene / alpha-olefin copolymer , ethylene / acrylate copolymer, low density polyethylene (LDPE), linear low density polyethylene Polyethylene (LLDPE), Medium Density Polyethylene (MDPE), or High Density Polyethylene The catalyst masterbatch may be a silicon-free ethylene-based polymer such as HDPE. The concentration of (B) in the mix is the maximum of the target concentration of (B) in the moisture-curable polyolefin formulation. The catalyst masterbatch may be a moisture-curing masterbatch having an amount (B) of more than 3 wt.%. The additional amount of (A) may be the same or different. By combining the amount of base polymer with various amounts of catalyst masterbatch, The masterbatch is used to produce moisture-curable polyolefins having various lower concentrations of (B). Other embodiments of the infusion formulations can be economically made.
[0024] The moisture curable polyolefin formulation consists essentially of components (A) and (B). This expression indicates that this embodiment of the moisture-curable polyolefin formulation comprises component (i). ~(x): (i) unsubstituted or substituted imidazole, (ii) unsubstituted or substituted polyester (iii) unsubstituted or substituted polyethers; (iv) unsubstituted or substituted ureas; (v) (vi) amine-carboxylates; (vii) amines (e.g., triethylamine). and ammonium compounds (e.g., triethyl ether chloride having the formula HN(CH2CH3)3Cl). (viii) metal carboxylates (where the metal is calcium, Any metal other than cobalt or zinc, or any metal other than cobalt or zinc metal), any seven of (ix)(i) to (viii), and (x)(i) to ( viii) each of the additional components selected from any one of For example, moisture curable polyolefin formulations may contain tin, Alternatively, it may further contain dibutyltin dilaurate, any one of or any Six, or each of (i) to (iv), (vi), (vii), and (viii) Alternatively, the moisture curable polyolefin formulation is tin-free and , or any six, or (i) to (iv), (vi), (vii), and (v iii) may not be included. "Additional components" refers to components that are intentionally introduced. Some of the components (i) to (x) may be the same as the components described above (e.g., component (A may be present as an impurity in or carried over from the synthesis of (e.g., an olefin polymerization catalyst carried over from the synthesis of (A) or a support resin), These impurities are inadvertently introduced into moisture-curable polyolefin formulations through moisture. Have a measurable, beneficial or detrimental effect on the performance of air-curable polyolefin formulations It is not expected that the moisture-curable polyolefin compound will have any of the components (i) to (x). Moisture cured polyolefin products, articles of manufacture, and articles made therefrom, if not also Coated conductors, as well as methods for making or using them, also contain the same components (i) to (x ) may not contain any of the components (A) and (B). Embodiments of the resistant polyolefin blend may include any component not expressly excluded above. Any such one or more structures not excluded above may further comprise one or more of the following: Examples of components are the optional additives (C) through (L).
[0025] The moisture curable polyolefin formulation comprises components (A), (B), and optionally , may be composed of zero, one or more additives (C) to (L). Moisture curable This embodiment of the polyolefin formulation excludes components not expressly included.
[0026] If an embodiment of the moisture curable polyolefin formulation does not contain a given component, it Articles containing or made from the same and articles not containing the same and made from the same Neither do polyolefin products contain it, nor articles containing it or made therefrom. nor does it include the methods of making or using it.
[0027] Moisture curable polyolefin formulations use Co,Zn(alkyl)acetate instead of (B). (Aza)carboxamidine or (aza)carboxamidine that does not contain thylacetonate Comparison of the moisture content of the samples containing either Co or Zn (alkyl) acetylacetonates without Co or Zn. They may be characterized by improved scorch resistance compared to air-curable polyolefin formulations. The scorch property is measured by the scorch time test method using a moving die rheometer (MDR) described later. , and (K)-1 calcium oxalate monohydrate, which is a moisture generating agent, was also added at 1.5% by weight. In some embodiments, the moisture curable polyolefin formulation comprises The moisture-curable polyolefin compound is (aza)carboxamidine / Co,Zn(aluminum) The molar ratio of acetylacetonate to acetylacetonate is 15:0.15 or 11:0.18. or 10.4:0.18, or 10.0:0.19, or 11:5.1. The composition may be characterized by improved scorch resistance when
[0028] An embodiment of the moisture curable polyolefin formulation may include Co,Zn(Al) instead of (B). (Aza)carboxamidine or (aza)carboxamide that does not contain acetylacetonate Contains either Co or Zn (alkyl) acetylacetonate that does not contain oxamidine Comparative moisture curable polyolefins made from comparative moisture curable polyolefin formulations Demonstration of a moisture-cured polyolefin product characterized by improved thermal creep resistance compared to conventional products. Moisture-curable polyolefin formulations that can be moisture-cured in embodiments, and compositions made therefrom Such an embodiment of the moisture-cured polyolefin product includes (K) a moisture generator. An embodiment of the moisture cured polyolefin product for thermal creep testing is , made by the tape extrusion and curing method described below. Moisture Cured Polyolefin The thermal creep resistance of such an embodiment of the product is determined by the thermal creep test method described below. To produce a moisture cured polyolefin product having improved thermal creep resistance. The moisture cured polyolefin formulations used for the present invention are 5:0.5, or 4:0.5. .00:0.9, or 3.00:0.95, or 2.40:0.95, or 2.40:1.6, or 2.30:0.99, or 1.74:1.01 (Aza ) Carboxamidine / Co,Zn (alkyl) acetylacetonate molar ratio obtain.
[0029] Moisture curable polyolefin compounds are characterized by (i) to (v): (i) Thermal creep test method As an average of three test pieces measured according to the method, after 20 minutes at 200°C, the 4%, or 50% to 150%, or 51% to 120%, or 55% to 94% (ii) thermal creep of 8.1 to 15.9 minutes, as measured according to the T90 crosslinking test method 90 cure times, (iii) Moisture cure test using a Moving Die Rheometer (MDR) When measured according to the test method, the maximum torque (MH) minus the minimum torque (ML) is obtained. (MH-ML) is 1.65 to 4.44 deciNewton meters (dN*m), or is 1.70~4.30dN*m, or 1.71~4.10dN*m, or 2.2 0 to 4.10 dN*m; (iv) any two of characteristics (i) to (iii); and (v) The test method may be characterized by any one of the characteristics (i) to (iii). More details will be provided later.
[0030] The moisture curable polyolefin formulation comprises components (A) and (B), and 0, 1 or more optional components.
[0031] Component (A) (hydrolyzable silyl group)-functional polyolefin prepolymer ("( A) a polyolefin moiety containing covalently bound condensation-curable silicon-containing groups. In this case, the polyolefin molecules are further polymerized via a water-based condensation cure to form polyolefins. By forming covalent siloxysilyl bridges between different chains of the polyolefin molecules, The resulting siloxysilyl bridges (Si-O-Si) bonded to carbon atoms of different chains At least one type of chain in the moisture-cured polymer product has more than one structural unit. (A) The polyolefin portion of the prepolymer is a polyethylene-based This is because the (A) prepolymer may have a main chain formed by polymerization of ethylene. Alternatively, the (A) prepolymer may be poly(ethylene-co-(C3- C 40 (A) the prepolymer may be ethyl olefin. The main chain is formed by copolymerization of olefin and at least one alpha-olefin. This means that...
[0032] (A) The prepolymer is prepared by the reaction of ethylene and an alkenyl-functional hydrolyzable silane. The alkenyl-functional hydrolyzable silane may be a copolymer of the formula (III) (R 2 ) m (R 3 ) 3-m Si-(C2-C6)alkenyl(III), m, R 2 , and R 3 are as defined above for formula (II). (C2-C6) Alkenyl can be vinyl, allyl, 3-butenyl, or 5-hexenyl. ) The prepolymer is a reactor copolymer of ethylene and vinyltrimethoxysilane. Vinyltrimethoxysilane is an alkenyl-functional hydrolyzable silane of formula (III) where subscript m is 3 and each R 2 (C1-C6) alkoxy(s (i.e., methoxy) and (C2-C6) alkenyl is vinyl (-C(H)=CH2) It is.
[0033] Alternatively, the (A) prepolymer may be a copolymer of ethylene and acetone, as described in US Pat. No. 6,936,671. The copolymer is a reactor copolymer of a fluoro-olefin and an alkenyl-functional hydrolyzable silane. It is possible.
[0034] Alternatively, the (A) prepolymer is typically a free radical such as a dialkyl peroxide. - Hydrolysis in a post-polymerization compounding or extrusion step promoted by a radical initiator The reaction of the silane with a degradable unsaturated silane (e.g., vinyltrimethoxysilane) results in grafting. and isolating the resulting silane-grafted polymer (e.g., S grafted thereto, such as polymers made by the IOPLAS™ process; is a homopolymer of ethylene having a carbon atom backbone with hydrolyzable silyl groups attached thereto. The grafted polymer may be for use in a subsequent processing step. The OPLAS™ process is described, for example, in US 3,646,155 and WO 2019 / 023363. The MONOSIL™ process is described, for example, in US Pat. 2016 / 0200843A1 and WO2019 / 005439A1 .
[0035] Alternatively, the (A) prepolymer may be a copolymer of ethylene and (C3-C 40 )Alpha-Olefin and unsaturated carboxylic acid esters (e.g., (meth)acrylate alkyl esters). ), in which case the copolymer may be a copolymer with one or more of SIOP Hydrolyzable polymers grafted thereto, such as those produced by the LAS™ process. It has a main chain having a silyl group.
[0036] Alternatively, the (A) prepolymer is typically a free radical such as a dialkyl peroxide. Hydrolysis during post-polymerization compounding or extrusion steps promoted by radical initiators grafting by reacting with a non-functional unsaturated silane (e.g., vinyltrimethoxysilane); The resulting silane-grafted polymer can be used immediately (without isolation) in a subsequent manufacturing step. ) in a process (e.g., the MONOSIL™ process) and hydrolyzable silanes such as alkenyl-functional hydrolyzable silanes of formula (III) It may be a mixture of a decomposable silane and a peroxide.
[0037] Alternatively, the (A) prepolymer may be SIOPLAS™ or MONOSIL™. Suitable for use in the ethylene and (C3-C 40 ) Alpha-olefins and and one or more copolymers of an aryl group and an unsaturated carboxylic acid ester of the formula (III) and a mixture of a hydrolyzable silane, such as an aryl-functional hydrolyzable silane, and a peroxide. Alpha-olefins are (C3-C 40 ) alpha-olefins, or (C 3-C 20 ) alpha-olefins, or (C3-C 10 ) alpha-olefin The alpha-olefin may have at least four carbon atoms (i.e., (C4) alpha-olefins or higher). (C3-C 10 )Alpha-Olefi Examples of olefins are propylene, 1-butene, 1-hexene, 1-octene, and 1-decene. Peroxides are described in WO2015 / 149634A1, page 5, line 6 to page 6, line 2. or (C1) an organic peroxide as described below with respect to organic peroxides. It is possible.
[0038] Alternatively, (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer (( A) prepolymers include (i) reactor copolymers of ethylene and hydrolyzable silanes, (i i) a mixture of ethylene, a hydrolyzable silane, and one or more alpha-olefins and unsaturated carboxylates; Reactor copolymers with carboxylic acid esters (e.g., US 6,936,671), (iii ) A homopolymer of ethylene having a carbon backbone and a hydrolyzable silane grafted to the carbon backbone. (iv) ethylenediaminetetraacetate (e.g., made by the SILOPAS™ process); and one or more alpha-olefins having a main chain and an unsaturated carboxylic acid ester. and a copolymer of a hydrolyzable silane grafted onto its backbone (e.g., SILOP (v) a polymeric olefin copolymer made by the ethylene / hydrolyzable silane / alkali process; Copolymers formed from mixtures with organic peroxides (e.g., MONOSIL™ Pro (vi) a mixture of ethylene and one or more alpha-olefins and from a mixture of an unsaturated carboxylic acid ester, a hydrolyzable silane, and an organic peroxide. Copolymers formed (e.g., made by the MONOSIL™ process) could be.
[0039] (A) The prepolymer is 79.0 to 99.99% by weight, or 85.0 to 99.9 9% by weight, or 90.0 to 99.99% by weight, or 95.0 to 99.99% by weight The moisture curable polyolefin formulation may be present in a concentration of If the composition further comprises at least one additive, the maximum amount of (A) is the moisture-curable polyisocyanate. 99.89% by weight, or 99.0% by weight, based on the total weight of the olefin blend. obtain.
[0040] Component (B) Condensation curing catalyst system (B) Condensation curing catalyst system is a 15:0.15 ratio of (A The molar ratio of (aza)carboxamidine to Co,Zn(alkyl)acetylacetonate is ) Contacting carboxamidine with Co,Zn(alkyl)acetylacetonate (B) or a moisture-curable polyolefin formulation comprising a mixture prepared by , not an (alkyl)acetylacetonate or (aza)carboxamidine anion It may be free of any organic anion.
[0041] (B) The condensation curing catalyst system is 15:0.15 (aza)carboxamidine / Co,Zn The molar ratio of (alkyl)acetylacetonates used is ) The number of moles of carboxamidine used Co,Zn (alkyl) acetylacetonate The range of 15 to 0.15 is 10:1 to 0.15:1 or can also be written as 10 / 1~0.15 / 1. (Aza)carboxamidine / Co,Zn The molar ratio of (alkyl)acetylacetonates is 11:0.18 or 10.4:0 .18, or 10.0:0.19, or 11:5.1, or 4.00:0. 9, or 3.00:0.95, or 2.40:0.95, or 2.40:1 It could be .6, or 2.30:0.99, or 1.74:1.01.
[0042] (B) The condensation curing catalyst system mixture is (B1) (aza)carboxamidine and Co, Zn Blends with (alkyl)acetylacetonates or (B2) (aza)carboxamides reaction products of the reaction of dimethyl with Co,Zn(alkyl)acetylacetonates, or (B3) The reaction product of (B2) and (aza)carboxamidine and / or Co, Zn ( The alkyl acetylacetonate may be in combination with an alkyl) acetylacetonate.
[0043] (B1) Blend is a mixture of carboxamidine and cobalt(alkyl)acetylacetoner. or blends of carboxamidines with zinc(alkyl)acetylacetonates. (B1) The blend may include a guanidine and cobalt ( Alkyl)acetylacetonate coordination complexes or guanidine and zinc(alkyl)acetylacetonate coordination complexes. The copolymer may include blends with alkyl (alkyl) acetylacetonate coordination complexes.
[0044] (B2) The reaction product is carboxamidine and cobalt(alkyl)acetylacetonate. The reaction products of carboxamidines and zinc(alkyl)amines (B2) may include the reaction product of a reaction with a cetylacetonate coordination complex: Reaction products from the reaction of guanidine with cobalt(alkyl)acetylacetonate coordination complexes. , or the reaction of guanidine with zinc(alkyl)acetylacetonate coordination complexes. The product may include
[0045] (B2) In preparing the reaction product, (aza)carboxamidine and Co,Zn(alanine) The reaction with acetylacetonate may be a proton exchange (acid-base) reaction. Alternatively, the reaction involves the neutral oxygen atom of the (alkyl)acetylacetonate of the relevant coordination complex. The first hybrid coordination complexes of Co or Zn were prepared by substituting (aza)carboxamidine. The first hybrid coordination complex may be a ligand exchange reaction to produce at least one A monodentate (alkyl) acetylacetonate ligand (anion) and at least one (aza Alternatively, the reaction may involve the reaction of (aza)carboxamidines. Addition of the coordinating complex to create a second hybrid coordination complex of Co or Zn and the second hybrid coordination complex is different from the first hybrid coordination complex. The second hybrid coordination complex contains two bidentate (alkyl)acetylacetonate ligands. and at least one (aza)carboxamidine ligand. Alternatively, the reaction may include any of the following: is a combination of two or more such reactions.
[0046] (B2) The reaction product has the formula M(L) x (Q) y and In the formula, M is a metal cation selected from Co(II), Co(III), and Zn(II). thione; the subscript x is an integer of 2 or 3 and is the formal oxidation state of the metal cation. each group L is independently equal to (alkyl)acetylacetonate, carboxamidine an anionic ligand which is an anion, or a guanidine anion; each group Q is independently a neutral ligand which is acetylacetone, carboxamidine, or guanidine; the subscript y is 0 to 3; at least one group L is a carboxamidine anion or or at least one group Q is a carboxamidine anion. More specifically, it is guanidine.
[0047] (B2) The reaction product is (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer. It may be preformed separately from the polymer (if not present). For example, (B2) may be a non- In a protic solvent, carboxamidine or guanidine is substituted with Co,Zn(alkyl)acetate. A reaction product (B2) is prepared in advance separately from (A) by contacting the reaction product with ethyl acetonate, and then (B2) the reaction product previously prepared in the above step and (A) a (hydrolyzable silyl group)-functional polyolefin They may also be combined with prepolymers to make moisture curable polyolefin formulations. Optionally, the aprotic solvent is added after the contacting step and before the combining step. The reaction product (B2) may be removed from the reaction product (B1) by distillation, evaporation, freeze-drying, or other suitable methods. The preparative step may be carried out by drying or stripping. The (B2) reaction product produced may be anhydrous and may optionally be free of aprotic solvents. Does not include.
[0048] Alternatively, the reaction product (B2) is a (hydrolyzable silyl group)-functional polyolefin. For example, (B2) may be prepared in situ in the presence of a fin prepolymer, but not both. However, (aza)carboxamidine or Co,Zn(alkyl)acetylacetonate (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer, can be prepared in situ by combining (aza)carboxamidine with (A) or a combination of Co,Zn(alkyl)acetylacetonate and (A) Then, the combination is converted to (aza)carboxamidine or Co,Zn(aza) (B) in the presence of (A) and 2) The reaction product can be prepared in situ.
[0049] (B2) Reaction product and (aza)carboxamidine and / or Co, Zn(alkoxy) (B3) is a combination of (aza) acetylacetonate. Carboxamidine and Co,Zn(alkyl)acetylacetonates in nonstoichiometric ratios. (B3) can be produced when the (B2) reaction product and excess (aza) are mixed in the same ratio. Co,Zn(alkyl)acetylacetoner may be combined with carboxamidine (B3) The combination (B2) is a mixture of the reaction product and excess Co,Zn(alkoxy) (aza)carboxamidine may be used in combination with (aza)acetylacetonate. (B3) is the reaction product of (B2) and (B1) (aza)carboxamidine and Co,Z It may be in combination with blends with n(alkyl) acetylacetonates.
[0050] (B) (aza)carboxamide of formula (I) or (II) of the condensation cure catalyst system embodiment Jin is the limit (i) ~ (x): (i) R 1 ~R 4 or R 5 ~R 9 At least one of Rui is each (C1-C 45 (ii) R is an alkyl group; 1 ~R 4 or R 5 ~R 9 At least one or only one of (C2-C 45 ) an alkenyl group; (iii )R 1 ~R 4 or R 5 ~R 9 At least one, or one or two of (C6-C 12 ) an aryl group; (iv) R 1 ~R 4 or R 5 ~R 9 At least one of Or one or two (C1-C 25 ) Alkyl-substituted (C6-C 12 ) an aryl group ;(v)R 1 ~R 4 or R 5 ~R 9 At least one, or one or two of (C 6-C 12 )Aryl-substituted (C1-C 25 (vi) R is an alkyl group; 1 ~R 4 Also is R 5 ~R 9 At least one or each of the following is an unsubstituted straight chain (C1-C5) alkyl: (vii) R 1 ~R 4 or R 5 ~R 9 Any two of the following together to form a (C1-C5) alkylene group, and the remaining R 1 ~R 4 or R 5 ~R 9 of At least one is independently as defined in any one of (i) to (vi). ;(viii)R 1 ~R 4 Any three of these or R 5 ~R 9 Any three of the following combined together and trivalent (C4-C10 ) forms an alkane triradical group, and the remaining R 1 ~R 4 or R 5 ~R 9 At least one of the following is independently defined as any one of (i) to (vi): (ix) R 1 ~R 4 Each of the bonds together form a tetravalent (C4-C 12 )a forming a leucane tetraradical group; and (x) R 5 ~R 9 Each of these is combined together to form 5 Valence (C5-C 14 ) forming an alkane penta radical group. obtain.
[0051] The (B) condensation cure catalyst system is substantially "Substantially pure" (B) can be characterized as being 90 to 100% by weight of the total of (B). 00% by weight, alternatively 95-100% by weight, alternatively 98-100% by weight, alternatively 90 , 95, or 98 to 99.99% by weight.
[0052] (B) The (aza)carboxamidine used in the condensation curing catalyst system is neutral (free base) or in the form of a protonic acid salt containing a protonic acid.
[0053] (B) Co,Zn(alkyl)acetylacetonate used in the condensation curing catalyst system , anhydrous form (no hydrates), or hydrated form. (Alkyl) acetylacetonates are effective in preventing scorch in moisture-curable polyolefin formulations. Scorch can be beneficially minimized during extrusion (e.g., This is the early moisture cure of moisture-curable polyolefin compounds (in the oven). The hydrated form of Kil) acetylacetonate is used to make moisture-curable poly(ethylene glycol) copolymers in anhydrous or low relative humidity environments. Further usefully serves as an in situ source of water molecules for moisture curing of olefin formulations There is a trade-off between minimizing scorch and allowing for in-situ moisture cure. The compound is a Co,Zn(alkyl)acetylacetonate in a moisture-curable polyolefin formulation. This can be accomplished by using (A) hydrate forms of the scorch retarders and (B) hydrate forms of the scorch retarders.
[0054] (B) The amount of condensation curing catalyst system used to prepare these mixtures is Equivalent to the sum of the amount of voxamidine and the amount of Co,Zn (alkyl) acetylacetonate The amount of (B) is 11.0 to 3.1% by weight of the moisture-curable polyolefin formulation, or 3.0 to 0.05% by weight, or 1.0 to 0.10% by weight (e.g., 0.15% by weight) It could be.
[0055] Optional Component (C) Peroxide: A compound that contains a carbon atom, a hydrogen atom, and two or more oxygen atoms. atom and has at least one -OO- group, provided that there are two or more -OO- When groups are present, each -OO- group is connected to another -OO- group via one or more carbon atoms. A molecule or an assembly of such molecules provided that they are closely bound to each other. (C) Peroxide The article comprises a moisture-curable polyolefin formulation comprising components (A), (B), and (C). (C) a moisture-curable polymer for curing, which comprises heating to a temperature above the decomposition temperature of a peroxide; It may be added to the polyolefin formulation.
[0056] The (C) peroxide may be a (C1) hydrocarbyl hydroperoxide. ) is the formula R O -OOH, where R O are independent, (C1-C 20 ) Alkyl group or (C6-C 20 ) an aryl group. 20 )Alkyl groups are Independently, unsubstituted or one or two (C6-C 12 ) substituted with aryl group Each (C6-C 20 The aryl group is unsubstituted or contains 1 to 4 (C 1-C 10 (C1) Hydroperoxides are substituted with 1,1-dialkyl groups. Methyl ethyl hydroperoxide, 1,1-dimethylpropyl hydroperoxide, Ben Zoyl hydroperoxide, tert-butyl hydroperoxide, tert-amyl hydroperoxide It may be cumyl hydroperoxide, or cumyl hydroperoxide. Cid is isopropyl cumyl hydroperoxide, t-butyl cumyl hydroperoxide , or cumyl hydroperoxide, or cumyl hydroperoxide (cumene hydroperoxide Peroxide, alpha, alpha-dimethylbenzyl hydroperoxide, CAS number The polysaccharide may be saccharide 80-15-9.
[0057] (C) The peroxide may be (C2) an organic peroxide. (C2) is of the formula R O -O.O. -R O where each R O are independently as defined above Alternatively, (C2) can be expressed as O -OOR a -OOR Ois the diperoxide of obtained, in the formula, R a is (C2-C 10 ) alkylene, (C3-C 10 ) cycloalkylene, or phenylene, and each R O are independently defined above (C2) Organic peroxides include bis(1,1-dimethylethyl) peroxide, bis( 1,1-Dimethylpropyl)peroxide, 2,5-Dimethyl-2,5-bis(1,1- Dimethylethylperoxy)hexane, 2,5-dimethyl-2,5-bis(1,1-dimethyl 4,4-bis(1,1-dimethylethylperoxy)hexyne, 4,4-bis(1,1-dimethylethylperoxy) Valeric acid, butyl ester, 1,1-bis(1,1-dimethylethylperoxy)-3,3 ,5-trimethylcyclohexane, benzoyl peroxide, tert-butyl peroxybenzoate di-tert-amyl peroxide ("DTAP"), bis(alpha-t-butyl (Isopropyl-peroxyisopropyl)benzene ("BIPB"), Isopropylcumyl t-butyl Cumyl peroxide, t-butyl cumyl peroxide, di-t-butyl peroxide, 2,5 -Bis(t-butylperoxy)-2,5-dimethylhexane, 2,5-bis(t-butyl 2,5-Dimethylhexyne-3,1,1-bis(t-butylperoxy) )-3,3,5-trimethylcyclohexane, isopropyl cumyl humyl peroxide, 4,4-Di(tert-butylperoxy)butylvalerate, or di(isopropyl The organic peroxide may be dicumyl peroxide, dicumyl peroxide, or dicumyl peroxide. It may be a peroxide.
[0058] A blend of two or more different (C) peroxides may be used.
[0059] At least one, or alternatively each (C) peroxide may contain one -OO- group.
[0060] The moisture curable polyolefin formulation may be free of (C) peroxide. The oxides, when present, are present in an amount of 0.01 to 4.5% by weight of the formulation of the present invention, or 0.05 It may be up to 2% by weight, alternatively 0.2-0.8% by weight.
[0061] Without being bound by theory, (C) the use of peroxide allows for a dual cure mechanism, Moisture cure of air-curable polyolefin formulations and moisture as a product of free radical cure It is believed that embodiments of cured polyolefin products result. Crosslinks can be formed between the water-decomposable silane groups, in which case the crosslinks are C-Si-O- Contains Si-C bonding motifs. (C) Peroxide-enabled free radical curing can form carbon-carbon bond bridges between the polymer chains of (A). Thus, a dual cure product is produced. The composition has a higher crosslink content than the moisture-cured only product and therefore have improved mechanical properties (e.g., modulus of elasticity, thermal creep performance) compared to the It is expected that this will happen.
[0062] Optional Components (Additives) (D) Scorch Retardants: Molecules that inhibit premature hardening; or aggregates of such molecules. Examples of scorch retarders are hindered phenols, semi-hydrides, Daled phenol, TEMPO, TEMPO derivatives, 1,1-diphenylethylene, 2 ,4-Diphenyl-4-methyl-1-pentene (alpha-methylstyrene dimer or (also known as AMSD), and US6277925B1, column 2, line 62 to column 3, line The allyl-containing compound is described in line 46. The olefin product may be free of (D). (D) Scorch retardant, if present, In all cases, the amount is 0.01 to 1.0% based on the total weight of the formulation and / or product of the present invention. It may be 5% by weight, or alternatively 0.1 to 1.0% by weight.
[0063] Optional Components (Additives) (E) Antioxidants: Organic molecules that inhibit oxidation; (E) Antioxidants are used in moisture-curable polyolefin formulations and and / or function to provide antioxidant properties to the crosslinked polyolefin product. An example of (E) is bis(4-(1-methyl-1-phenylethyl)phenyl)amine (e.g. For example, NAUGARD 445), 2,2'-methylene-bis(4-methyl-6-t-butyl Phenol) (e.g., VANOX MBPC), 2,2'-thiobis(2-t-butyl -5-Methylphenol (CAS number 90-66-4, 4,4'-thiobis(2-t-butyl)phenol 4,4'-thiobis(6-tert-butyl-m-cre Also known as ZOLL, CAS number 96-69-5, commercially available LOWINOX TB M-6, 2,2'-thiobis(6-t-butyl-4-methylphenol (CAS no. 9 0-66-4, commercially available LOWINOX TBP-6), tris[(4-tert-butyl -3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2 ,4,6-trione (e.g., CYANOX1790), pentaerythritol tetrakis bis(3-(3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)propionate onate) (e.g., IRGANOX1010, CAS number 6683-19-8), 3, 5-Bis(1,1-dimethylethyl)-4-hydroxybenzenepropanoic acid 2,2'-thio Odiethanediyl esters (e.g., IRGANOX1035, CAS number 41484- 35-9), distearyl thiodipropionate ("DSTDP"), dilauryl thiodi Propionate (e.g., IRGANOX PS800), stearyl 3-(3,5-di -t-butyl-4-hydroxyphenyl)propionate (e.g., IRGANOX10 76), 2,4-bis(dodecylthiomethyl)-6-methylphenyl (IRGANOX1 726), 4,6-bis(octylthiomethyl)-o-cresol (e.g., IRGAN OX1520), and 2',3-bis[[3-[3,5-di-tert-butyl-4- Hydroxyphenyl]propionyl]propionohydrazide (IRGANOX1024 (E) is 4,4'-thiobis(2-t-butyl-5-methylphenol) ( Also known as 4,4'-thiobis(6-tert-butyl-m-cresol), 2,2'-thiobis(6-t-butyl-4-methylphenol, tris[(4-tert -Butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-trimethyl Diene-2,4,6-trione, distearyl thiodipropionate, or dilauryl thiodipropionate, or a combination of any two or more thereof. The compound is tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl )Methyl]-1,3,5-triazine-2,4,6-trione and distearyl thiodipropionate Moisture curable polyolefin compound and / or crosslinked polyolefin The olefin product may be free of (E). (E) Antioxidants, if present, act as humectants. of the total weight of the air-curable polyolefin compound and / or crosslinked polyolefin product. It may be 0.01 to 1.5% by weight, or alternatively 0.1 to 1.0% by weight.
[0064] Optional Component (F) Tree Retardant: Suppresses water and / or electrical trees A tree retarder is a molecule, or an aggregate of such molecules. A tree retarder is a water tree retarder or an electrical tree retarder. Water tree retarders can be used as retarders for water trees exposed to the combined effects of an electric field and moisture or water. It is a compound that inhibits water treeing, a process that causes polyolefins to deteriorate when exposed to electrical current. Tree retardation is an electrical pre-decomposition process in solid electrical insulation caused by partial discharge. It is a compound that inhibits electrical trees. Electrical trees can occur in the absence of water. Trees and electrical trees are electrical trees that contain coated conductors, the coating of which contains polyolefin. This is a question about cables. (F) is poly(ethylene glycol) (PEG). The polyolefin composition and the crosslinked polyolefin product may be free of (F). (F) The tree retarder may be present in an amount of 0.01 to 1 based on the total weight of the composition of the present invention. It may be 0.5% by weight, or alternatively 0.1-1.0% by weight.
[0065] Optional Component (Additive) (G) Colorant, e.g., a pigment or dye. For example, Carbon black or titanium dioxide. Carbon black is a poly(1-butene-co-ene) (ethylene) copolymer (≧95% by weight to less than 100% by weight of the total weight of the masterbatch) and carbon black (composition of 0% by weight or more to ≦5% by weight or less of the total weight of the masterbatch) The carbon black may be provided as a carbon black masterbatch, which is a mixture of It is a microcrystalline form of paracrystalline carbon with a high surface area to volume ratio, but lower than that of activated carbon. Examples of carbon black include furnace carbon black, acetylene carbon black, Conductive carbon (e.g., carbon fiber, carbon nanotube, graphene, graphene) graphite, and expanded graphite platelets). Moisture-curable polyolefin formulations and The crosslinked polyolefin product may be free of (G). If present, it may be present in an amount of from 0.1 to 35% by weight, alternatively from 1 to 10% by weight, of the formulation of the invention.
[0066] Optional Component (Additive) (H) Moisture Scavenger. (H) Moisture Scavenger is a moisture curing agent. In this case, the premature moisture cure of the polymeric polyolefin compound is inhibited. The degradation can be caused by early or prolonged exposure of moisture curable polyolefin formulations to ambient air. Examples of (H) are octyltriethoxysilane and octyltrimethoxysilane. Moisture-curable polyolefin formulations and / or crosslinked polyolefin products (H) may be absent. (H), when present, constitutes 0.001 of the formulation of the present invention. It may be from 0.01 to 0.10% by weight.
[0067] Optional Components (Additives) (I) Hindered Amine Light Stabilizer: At least one Basic nitrogen that binds to the sterically bulky organic group and acts as an inhibitor of degradation or decomposition A molecule containing an atom or an assembly of such molecules. (I) is a sterically hindered amino A polyolefin composition having a functional group, suppressing oxidative deterioration, and containing (C) an organic peroxide. Examples of suitable (I) compounds are compounds that can increase the shelf life of embodiments of the product. Tanedioic acid dimethyl ester, 4-hydroxy-2,2,6,6-tetramethyl-1-piperidine Lysine-ethanol (CAS number 65447-77-0, commercially available LOWILITE62) and N,N'-bisformyl-N,N'-bis(2,2,6,6-tetramethyl-N,N'-dimethyl-N,N'-dimethyl- tetramethyl-4-piperidinyl)-hexamethylenediamine (CAS number 124172- 53-8, commercially available Uvinul 4050 H). The formulations and products of the present invention are (I) The hindered amine stabilizer, when present, is 0.001 to 1.5% by weight of the composition, or 0.002 to 1.0% by weight, or 0 It may be between .05 and 1.0% by weight.
[0068] Optional Components (Additives) (J) Processing Aids: Used in manufacturing equipment such as extruders and dies Molecules that reduce adhesion of polymer melts in the polymer melt and reduce melt fracture of materials. (J) is a full Polyorganopolymers, polyorganosiloxanes, metal salts of fatty carboxylic acids, fatty carboxamides , waxes, ethylene oxide (co)polymers, and non-ionic surfactants. The formulations and products of the present invention may be free of (J). (J) Processing aids are not present. If present, it may be present in an amount of from 0.05 to 5% by weight of the formulation of the present invention.
[0069] Optional Components (Additives) (K) Moisture Generators: (a) Release water molecules when heated or (b) a hydrate molecule that decomposes when heated to produce water molecules (as a by-product). Molecules of potential water sources. (K)(a) is a group 1 or (K)(b) can be in the form of a hydrate of a Group 2 metal oxalate. and a mixture thereof which generates water when heated. The product may not contain (K). (K) The moisture generating agent, when present, is a component of the composition of the present invention. The amount may be 0.5 to 2.5% by weight, or 1.0 to 1.9% by weight of the mixture.
[0070] The formulations and / or products of the present invention are useful in the preparation of lubricants, mineral oils, antiblocking agents, metal Deactivators (e.g., oxalyl bis(benzylidene)hydrazide (OABH)), auxiliary agents , nucleating agents, or flame retardants.
[0071] Any optional component may have at least one characteristic or property, It may be useful to impart to the formulations and / or products of the invention the following characteristics: The properties are advantageous in applications where the formulations and / or products of the invention are exposed to high operating temperatures. These may be useful in improving the performance of the formulations and / or products of the invention in other applications. Such operations or applications include melt mixing, extrusion, molding, hot water pipes, and power cables. The insulating layer of the filter is included. chemicals
[0072] Any compound herein includes naturally occurring and / or isotopically enriched forms. Isotopically enriched forms may be used for further purposes, such as for medical or anti-counterfeiting purposes. The present invention may have further applications.
[0073] Any compound, chemical composition, formulation, material, or product herein may contain H, Li , Be, B, C, N, O, F, Na, Mg, Al, Si, P, S, Cl, K, Ca, Sc , Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, B r, Rb, Sr, Y, Zn, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, I, Cs, Ba, Hf, Ta, W, Re, Os, Ir, Pt, Au, Selected from the group consisting of Hg, Tl, Pb, Bi, lanthanides, and actinides It is not necessary to include any one of the chemical elements, provided that the chemical elements required for them (e.g. , C and H) necessary for polyolefins are not excluded.
[0074] Each (C1-C 45 ) The hydrocarbyl groups are independently (C1-C 45 ) alkyl group, (C2-C 45 ) alkenyl group, (C6-C 12 ) aryl groups, (C1-C 25 ) Alki substitution (C6-C 12 ) an aryl group, or (C6-C 12 )Aryl substituted (C1-C2 5) It can be an alkyl group.
[0075] Each (C1-C 45 ) The hydrocarbylene groups are independently (C1-C 45 ) Alkylene group, (C2-C 45 ) alkenylene group, (C6-C 12 ) arylene group, (C1-C 25 ) Alkyl-substituted (C6-C 12 ) an arylene group, or (C6-C 12 )Aryl-substituted ( C1-C 25 ) alkylene groups.
[0076] Each of the trivalent, tetravalent, and pentavalent (C1-C 45)Hydrocarbons are each independently: (C 1-C 45 ) Alkanes, (C2-C 45 )Alkenes, (C6-C 12 ) arene, (C1 -C 25 ) Alkyl-substituted (C6-C 12 ) arene, or (C6-C 12 ) Aryl Exchange(C1-C 25 ) may be a trivalent, tetravalent, or pentavalent derivative of an alkane.
[0077] Each (C1-C 45 ) hydrocarbyl groups, (C1-C 45 ) Hydrocarbylene, trivalent (C1-C 45 ) Hydrocarbons, tetravalent (C1-C 45 ) hydrocarbons, and pentavalent (C1-C 45 ) Hydrocarbons are independently unsubstituted or halogen, unsubstituted (C1-C6 ) alkyl, -NH2, -N(H)(unsubstituted (C1-C6) alkyl), -N(unsubstituted ( From -O(unsubstituted (C1-C6) alkyl), -OH, and -O(unsubstituted (C1-C6) alkyl) Substituted with 1 to 5 independently selected substituents.
[0078] Substitution means that one or more carbon-bonded hydrogen atoms (H atoms of CH) have been replaced with an equal number of independently selected Formally substituted with the selected substituents (one substituent per H atom of CH) up to Each substitution (including one substitution) means that one or more carbon-bonded substituents are formed, All H atoms of CH are replaced by substituents;
[0079] "Unsubstituted" means that the atoms consist of carbon and hydrogen atoms.
[0080] The unsubstituted (C1-C6) alkyl is independently straight chain, branched chain, or cyclic (unsubstituted ( (C1-C6)alkyl).
[0081] An unsubstituted (C3) alkyl group is a monovalent radical of the formula C3H7 Examples are -CH2CH2CH3 and -CH(CH3)2. Unsubstituted (C4) alkyl A aryl group is a monoradical of formula C4H9. Examples are -CH2CH2CH2CH3, -CH( CH3)CH2CH3, -C(CH3)2CH3, -CH2CH(CH3)CH3, and and -C(CH3)3. An unsubstituted (C5) alkyl group has the formula C5H 11 With monoradical Examples are -CH2CH2CH2CH2CH3, -CH(CH3)CH2CH2CH3 , -C(CH3)2CH2CH3, -CH2CH(CH3)CH2CH3, -CH2C( CH3)2CH3, -CH2CH2CH(CH3)CH3, -CH(CH2CH3)2, and -CH2C(CH3)3. An unsubstituted (C6) alkyl group has the formula CH 13 Things It is a radical. Examples are -CH2CH2CH2CH2CH2CH3, -CH(CH3)C H2CH2CH2CH3, -C(CH3)2CH2CH2CH3, -CH2CH(CH3 )CH2CH2CH3, -CH2C(CH3)2CH2CH3, -CH2CH2CH(C H3)CH2CH3, -CH2CH2C(CH3)2CH3, -C(CH3)(CH2C H3)2, and -CH2CH2C(CH3)3.
[0082] (Alkyl) acetylacetonates: unsubstituted or alkyl-substituted acetylacetones Monoanionic derivative (conjugate base). Unsubstituted acetylacetone has the formula CH3C(=O)CH 2C(=O)CH3 and the enolate of formula CH3C(=O)CHC(OH)CH3 Unsubstituted acetylacetonates include the acetylacetonates of the formula CH3C(=O)CH=C(O-) It is drawn as the enolate of CH3 and mono-deprotonates unsubstituted acetylacetone. Alkyl-substituted acetylacetones are made formally by the following formula: The unsubstituted acetyl group can be obtained by replacing the H atom with an alkyl group such as Ra as defined above. Formally derived from acetone. Alkyl-substituted acetylacetonates are alkyl-substituted It is formally prepared by mono-deprotonating acetylacetone.
[0083] Carboxamide: A compound having a pentavalent functional group of the formula CC(=O)-N. The group is not part of a heteroaromatic ring. Also known as an amide.
[0084] Carboxamidine: a compound having a hexavalent functional group of the formula NC(=N-)-C, The functional group is not part of a heteroaromatic ring. Also known as amidine.
[0085] Guanidine: A compound having a pentavalent functional group of the formula NC(=N-)-N. is not part of a heteroaromatic ring.
[0086] Organic anion: A negatively charged ion of a hydrocarbon or heterohydrocarbon. ) may be present at one or more atoms independently selected from carbon, nitrogen, oxygen, and sulfur. For example, in 1-methylethoxide (the anion of 2-propanol), the negative charge is In unsubstituted acetylacetone (anion of unsubstituted acetylacetone), The negative charge resides partially on the two oxygen atoms and partially on the C-3 carbon atom.
[0087] Protic Acid: Independently, HCl, HBr, HI, acetic acid, or methanesulfonic acid. definition
[0088] Alternatively, it may precede a different embodiment.
[0089] Ambient or room temperature: 23°C ±1°C unless otherwise stated.
[0090] Aspects: embodiments of the invention. "Some aspects" and the like include numbered and unnumbered aspects. Qualify.
[0091] ASTM: Standards Organization, ASTM International (West Cons Hohocken, Pennsylvania, USA).
[0092] The comparative examples are used for comparison purposes and should not be considered prior art.
[0093] Not containing or lacking means completely absent or undetectable. This means:
[0094] IEC: Standards Organization, International Electrotechnical Commission, Geneva, Switzerland.
[0095] IUPAC stands for International Union of Pure and Applied Chemistry (IUPAC Secretariat (R esearch Triangle Park,North Carolina,USA )).
[0096] Masterbatch: A concentrated mixture of additives dispersed in a carrier resin.
[0097] May is not a requirement but confers the ability to choose.
[0098] Generalized format "Metal(Roman numerals)" (e.g. "Cobalt(II)" or "Co(III)"), Roman numerals (e.g., (II) or (III)) , the formal oxidation state (e.g., +2 or +3) of the metal (e.g., cobalt or Co) show.
[0099] Effective: Functionally capable or effective.
[0100] Optional (optionally): Not existing (or excluded); or To be present (or contained).
[0101] PPM or Parts Per Million: By weight unless otherwise stated.
[0102] Properties: Measured using standard test methods and known conditions unless otherwise stated. will be done.
[0103] Ranges include endpoints, subranges, and integer and / or fractional values within them. However, the range of integers does not include decimal values.
[0104] Density: ASTM D792-13, Density and specific gravity of plastics by displacement (relative Standard Test Method for Density, Method B (Density in Liquids Other Than Water, e.g., Liquid 2-Propanol) The mass of grams per cubic centimeter is measured according to the 100 g / cm2 (for testing plastics). Units (g / cm 3 ).
[0105] Melt Index "I2": 190°C / 2, formerly known as "Condition E". Measured according to ASTM D1238-13 using 16 kg load. Unit of grams per 10 minutes (g / 10 min). EXAMPLES
[0106] Carboxyamidine Compounds: 1,8-Diazabicyclo[5.4.0]undeca-7- 1,5-Diazabicyclo[4.3.0]non-5-ene (DBU) and 1,5-Diazabicyclo[4.3.0]non-5-ene (DBN) Obtained from TCI Shanghai, China.
[0107] Guanidine Compounds: Tetramethylguanidine (TMG). TCI Shangha Obtained from i,China.
[0108] Co,Zn(alkyl)acetylacetonate compounds: Co(II)(acac)2 , Co(III)(acac)3, and Zn(II)(acac)2. Each acac is 2 ,4-pentanedionate. Obtained from TCI Shanghai, China.
[0109] High density polyethylene 1 (HDPE1): Density is 0.965g / cm 3 , Melt Inde High density polyethylene homopolymer with a modulus (I2) of 8g / 10min.
[0110] (Hydrolyzable silyl group)-functional prepolymer (A)-1: 98.5% by weight of ethyl Reactor copolymer of ethylene and 1.5 wt. % vinyltrimethoxysilane. Free radical The initiator was used to react ethylene and vinyltrimethoxysilane in a tubular high pressure polyethylene reactor. The Dow Chemical Company Available from ny as SI-LINK(TM) DFDA-5451.
[0111] Condensation curing catalyst system (B)-1: DBU / Co(II)(acac)2 molar ratio of 2.0 : 1.0, an in situ prepared mixture of DBU and Co(II)(acac)2.
[0112] Condensation curing catalyst system (B)-2: The molar ratio of TMG / Zn(II)(acac)2 is 2.3 : 1.0, an in situ prepared mixture of TMG and Zn(II)(acac)2.
[0113] Condensation curing catalyst system (B)-3: DBU / Zn(II)(acac)2 molar ratio is 1.7 : 1.0, an in situ prepared mixture of DBU and Zn(II)(acac)2.
[0114] Condensation curing catalyst system (B)-4: DBN / Zn(II)(acac)2 molar ratio is 2.1 : 1.0, an in situ prepared mixture of DBN and Zn(II)(acac)2.
[0115] Condensation curing catalyst system (B)-5: DBU / Zn(II)(acac)2 molar ratio 1:1 A preformed mixture of DBU and Zn(II)(acac)2, in which Zn (II) A measured volume of anhydrous 2-(acac)2 sufficient to make a 0.1 molar solution. In tetrahydrofuran (THF), measured amounts of DBU and Zn(II) (acac )2. Heat the solution at 60°C for 3 hours. The volatiles (THF) are removed to give (B)-5.
[0116] Condensation curing catalyst system (B)-6: DBU / Zn(II)(acac)2 molar ratio 2:1 A preformed mixture of DBU and Zn(II)(acac)2, where Zn(II) (B)-5 was prepared in advance, except that twice as much DBU was used as in (acac)2. The fluororesin may be prefabricated according to the method used to prepare the fluororesin.
[0117] Condensation curing catalyst system (B)-7: DBU / Zn(II)(acac)2 molar ratio of 1.7 : 1.0, an in situ prepared mixture of DBU and Zn(II)(acac)2.
[0118] Condensation curing catalyst system (B)-8: DBU / Zn(II)(acac)2 molar ratio of 2:1 , an in situ prepared mixture of DBU and Zn(II)(acac)2.
[0119] Condensation curing catalyst system (B)-9: DBU / Co(II)(acac)2 molar ratio of 2.0 : 1.0, an in situ prepared mixture of DBU and Co(II)(acac)2.
[0120] Condensation curing catalyst system (B)-10: DBU / Co(III)(acac)3 molar ratio of 1 :1, an in situ prepared mixture of DBU and Co(III)(acac)3.
[0121] Condensation curing catalyst system (B)-11: DBU / Co(III)(acac)3 molar ratio of 2 A mixture of DBU and Co(III)(acac)3 with a ratio of 0.0:1.0 was prepared in situ. Compound.
[0122] Condensation curing catalyst system (B)-12: The molar ratio of DBU / Zn(II)(acac)2 is 5. A mixture of DBU and Zn(II)(acac)2, 0:1.0, prepared in situ .
[0123] Condensation curing catalyst system (B)-13: The molar ratio of DBU / Zn(II)(acac)2 is 0. An in situ mixture of DBU and Zn(II)(acac)2, 19:1.0 thing.
[0124] Condensation curing catalyst system (B)-14: DBU / Zn(II)(acac)2 molar ratio of 10 An in situ mixture of DBU and Zn(II)(acac)2 at 0.0:1.0 thing.
[0125] Comparative condensation curing catalyst system (B)-15: DBU / Zn(II)(acac)2 molar ratio The in situ mixture of DBU and Zn(II)(acac)2 with a ratio of 0.10:1.0 Mixtures (comparison for molar ratios).
[0126] Each acac in (B)-1 to (B)-15 is an unsubstituted acetylacetonate (i.e. , 2,4-pentanedionate).
[0127] Antioxidant (E)-1: Pentaerythritol tetrakis(3-(3,5-bis(1 ,1-dimethylethyl)-4-hydroxyphenyl)propionate (e.g., IRGA NOX 1010, CAS number 6683-19-8; BASF)
[0128] Antioxidant (E)-2: 2',3-bis[[3-[3,5-di-tert-butyl- 4-Hydroxyphenyl]propionyl]propionohydrazide (IRGANOX 1 024;BASF).
[0129] Moisture Generator (K)-1: Calcium oxalate monohydrate. Moving die rheometer It is used as the water source for hardening experiments carried out using the (MDR) instrument. Part A: (K)-1 Formulations containing moisture generators
[0130] Method 1 for formulating moisture-curable polyolefin compounds: HAAKE mixer (Thermo Fisher Scientific), (A) (hydrolyzable silyl group)-functional A polyolefin prepolymer (e.g., ((A)-1)) is heated at 120°C and 0 revolutions per minute (rp Melt at 120°C for 5 minutes at 45 rpm, then at 120°C for 2.5 minutes at 45 rpm. (B) is added to (A) quickly. For example, first add Co(II)(ac ac)2 was added, followed by the addition of DBU to prepare (B)-1 in situ. First, Zn(II )(acac)2 is added, then TMG is added to prepare (B)-2 in situ. First, Z Add n(II)(acac)2 followed by DBU to generate (B)-3 in situ; Zn(II)(acac)2 was added first, followed by DBN to prepare (B)-4 in situ. (B)-5 is added to the mixture, or (B)-6 is added to the mixture. Mix the contents at 120°C and 45 rpm for 1 minute. If necessary, (K) Moisture generation Add the agent (e.g., (K)-1) in small portions and then mix for 2 minutes at 120°C and 45 rpm. Continue mixing. Remove the material from the mixer and press the samples according to the plaque preparation test method. This causes plaque formation.
[0131] Plaque Preparation Test Method: Materials from Preparation Method 1 of Moisture-Curable Polyolefin Compounds The samples were pressed at 120°C and 0.5 megapascals (MPa) for 20 seconds to form plaques. The thickness of the plaque is determined by the following formula: In particular, the degree of scorching of the compound during its preparation (e.g., in a HAAKE mixer). This may vary depending on the application.
[0132] Moisture cure test method using a moving die rheometer (MDR): Moisture cure polymers A 4.5 gram sample of the material obtained from Preparation Method 1 of the polyolefin formulation was prepared according to ASTM According to D5289-17 (Standard test method for rubber vulcanization using rotorless cure meter) The plaques prepared according to the plaque preparation test method were used. The minimum torque (ML) at 180°C is measured using the MDR and the following procedure. Bing die rheometer (MDR) instrument MDR2000 (Alpha Technology gies), the test specimen was heated at 180°C for 20 minutes, 100 cycles per minute (cpm; 1.67 Hertz (Hz)) to monitor the change in torque with a vibration deformation of 0.5 arc degrees The minimum torque value measured is called "ML" in deciNewton meters (dN*m). ML indicates the degree of pre-curing of the formulation during the plaque preparation test method, and MDR This is the starting point of the moisture curing of the present invention using the above. As the moisture curing (crosslinking) of the present invention progresses, The measured torque value increases and eventually reaches the maximum torque value. We denote the torque value as "MH" expressed as dN*m. All other things being equal, the MH torque The higher the torque value, the greater the degree of cross-linking. All else being equal, the torque value The shorter the time it takes for the test specimen to go from ML to 1 lb / in (1.1 dN*m), the better the test specimen. The hardening rate is fast. Conversely, the torque value from ML to 1 lb / in (1.1 dN*m) The longer the time required to cure, the slower the test specimen will cure. ML is the rheological -Changes in viscosity, and a higher value indicates a higher degree of crosslinking. ML=1.0 lbf.in(1. Record the cure time required to reach 1.00 lb / i n=0.113 Newton meters (N*m).
[0133] Scorch Time Test Method. This method is used to test moisture-curable polyolefins prepared as pellets. Characterize the scorch resistance of the fin compound. Scorch resistance is determined by the MDR. The minimum torque (ML) measured at 180°C using the moisture cure test method used is 1 pound The length of time it takes to increase the torque by lb / in (ts) 1 (1.0 lb / in = 1.1 dN*m). 1.00 lb / in = 0.113 nu The longer the ts1 time, the better the scorch resistance (scorch retardation). The moisture curable polyolefin formulation advantageously exhibits a high degree of thermal expansion (also known as thermal expansion coefficient) of 180°C. It can be characterized by its resistance to scorch at ℃ (MDR ts1) 8 to 16 minutes of scorch Measured according to the MDRts1 time test method. If a sample exhibits scorch resistance according to this MDRts1 method, To say, the maximum torque (MH) value measured is greater than the minimum torque (ML) value measured. Must be at least 1.0dN*m higher (i.e., MH-ML ≥ 1.0dN If MH-ML<1.0dN*m, the sample is not scorch resistant. It is characterized by:
[0134] T90 cure time test method. This method measures the cure rate as the time required to reach 90% cure. The T90 crosslinking time was characterized as the time (min) required for crosslinking using the MDR. 9. The minimum torque (ML) and maximum torque (MH) measured at 180°C using the moisture cure test method This is the length of time it takes to increase the torque to 0% (0.90 MH).
[0135] Comparative Examples 1 to 5 (CE1 to CE5): Comparative formulations were prepared using moisture generating agent (K)-1. and tested according to the methods described above, see results in Table 1 below.
[0136] Examples 1 to 10 of the invention (IE1 to IE10): Using the moisture generating agent (K)-1 Moisture curable polyolefin formulations were prepared and tested according to the methods described above. See results in Table 3 and 4.
[0137] [Table 1]
[0138] [Table 2]
[0139] [Table 3]
[0140] As shown in Table 1, the comparative formulations exhibited substantially lower maximum torque values, as indicated by MH. As shown in Tables 2 and 3, the formulations of the present invention showed poor curing as expected. have a significant degree of cross-linking as indicated by the qualitatively larger maximum torque value MH Furthermore, the formulations of the present invention generally had faster cure rates and Therefore, the cured product can be obtained in a shorter time, as indicated by the shorter T90 cure time. It was created. Part B: (K) Formulations that do not contain (lack) a moisture generating agent.
[0141] Preparation of catalyst masterbatches 1 to 5 (invention). Braben The mixture was then placed in a Brabender GmbH & Co KG mixer until it was completely melted. Add HDPE1 to the melt. Add antioxidants (E)-1 and (E)-2 to the melt. Next, Then, add (B) the condensation curing catalyst system. For example, first add Zn(II)(acac)2. Then DBU is added to prepare (B)-7 in situ. First, Zn(II)(acac) Add 2 and then DBU to prepare (B)-8 in situ. First, add Co(II)(a (B)-9 was prepared in situ by adding Co(I II) Add (acac)2, then add DBU, and mix (B)-10 or (B)-11. Either make each one on the spot, or (predictive) add pre-made (B)-5 or by adding pre-prepared (B)-6 to obtain a catalyst matrix from a pre-prepared condensation curing catalyst system. A star batch is made. The resulting formulation is mixed for 2 minutes at 155°C and 45 rpm. The mixture was removed from the mixer and tested by hot pressing using the plaque preparation test method. The material is formed into plaques. The plaques are cut into small pellets. The pellets are fed into a single-screw extruder. and feed the moisture-curing polyolefins as catalyst master batches 1, 2, 3, 4, and 5, respectively. Prepare small pellets of the olefin compound. Catalyst Masterbatches 1 to 5 are 3.33 weight percent. % by weight of antioxidant (E)-1 and 1.67% by weight of antioxidant (E)-2, and 0.6 wt. % (B) of the condensation cure catalyst system (B)-7, (B)-8, (B)-9, (B)-10 or (B)-11, respectively.
[0142] Comparative master batches 1 to 4 were prepared using the same procedure as catalyst master batch 1. However, instead of 2.6 wt. % of the (B)-7 condensation cure catalyst system, a comparative master Batches 1-4 contained the following components Zn(II)(acac)2, DBU, Co(II)( Co(III)(acac)2, and Co(III)(acac)3 were each mixed at 1 It contained .3% by weight.
[0143] Tape extrusion and curing methods: measured quantities with a weight / weight ratio of 5.8 / 94.2 respectively Catalyst Masterbatch 1 (see Preparation of Catalyst Masterbatch 1) and (Hydrolyzable Silica The (hydroxyl group)-functional prepolymer (A)-1 is dry blended in a vinyl bag. The liquid blend was fed into a single screw extruder operating at 160°C and 45 rpm to produce a moisture-curing polymer. The polyolefin blend is extruded as a 1 mm thick tape having a width of about 3.5 mm. The mixture does not contain (K) a moisture generating agent. Then, the extruded tape is "Dog-bone" shaped specimens were cut and immersed in a 90°C water bath for 3 hours. The test specimens are cured to produce examples of moisture cured polyolefin products of the present invention. The thermal creep of moisture cured polyolefin products is measured according to the RAFT test method.
[0144] Thermal Creep Test Method. Moisture-cured polymers prepared by tape extrusion and cure method To measure the degree of crosslinking, and therefore the degree of cure, in test samples of polyolefin products. ASTM D2655-17 (Cross-Linking for Wire and Cable Rated 0-2000V) 20 Newtons per square centimeter (N / c) in accordance with the standard for polyethylene insulation m 2 ) and hardened (3 hours in 90°C water bath) test specimens ((K ) without moisture generator) are subjected to thermal creep. After 20 minutes, the final length is measured. The length of the tested specimen is then measured as it cools. The amount of elongation divided by the initial length is the thermal creep. The degree of elongation of the test specimen is measured as a percentage of the elongation of the test specimen before the thermal creep condition. It is expressed as a percentage (%) of the length of the test specimen after the thermal creep condition relative to the initial length. The lower the thermal creep percentage, the less the test specimen will elongate under load, and therefore The lower the thermal creep value, the greater the degree of crosslinking and therefore the greater the degree of hardening. , suggesting a high degree of cross-linking.
[0145] Comparative Examples 6 to 9 (CE6 to CE9): Comparative formulations are Comparative Masterbatch 1 ~4 different from each other, does not contain the moisture generating agent (K), and is prepared according to the above method. were tested, see results in Table 4 below.
[0146] Examples 11 to 15 (IE11 to IE15) of the present invention: Moisture-curable polyolefins of the present invention Each of the blends was prepared from a different one of the catalyst masterbatches 1 to 5. The moisture generating agent (K) was not included and the test was performed according to the above method. The results are shown in Table 5 below. Please refer to.
[0147] [Table 4]
[0148] [Table 5]
[0149] As shown in Table 4, the comparative formulation appeared to have minimal or no crosslinking as indicated by fracture of all specimens in less than 1 minute (extension at break is very long) and therefore failed to provide a cured product. As shown in Table 5, the inventive formulation provided an inventive cured product with substantially greater crosslinking as indicated by the fact that all specimens remained intact after 20 minutes at 200°C and the thermal creep values were substantially less than 100%. The lower the % thermal creep, the greater the degree of crosslinking, and the greater the degree of crosslinking, the more suitable the moisture cured polyolefin product will be for use as a jacketing layer for power cables. The present invention includes the following aspects. Section 1. 1. A moisture curable polyolefin formulation comprising: (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer; (B) a condensation cure catalyst system comprising a mixture made by contacting a compound which is a carboxamidine or guanidine, either unsubstituted or substituted (collectively referred to as an "(aza)carboxamidine"), with a compound which is a cobalt acetylacetonate coordination complex or a zinc acetylacetonate coordination complex, each acetylacetonate independently being unsubstituted or substituted with 1 to 5 alkyl groups, each alkyl group being unsubstituted (collectively referred to as a "Co,Zn(alkyl)acetylacetonate"), wherein the Co,Zn(alkyl)acetylacetonate is selected from cobalt(II)((alkyl)acetylacetonate)2, cobalt(III)((alkyl)acetylacetonate)3, and zinc(II)((alkyl)acetylacetonate)2; the amount of (A) is 79.0 to 99.99 weight percent (wt%) and the amount of (B) is 21.0 to 0.01 wt% of the moisture-curable polyolefin formulation, The moisture-curable polyolefin formulation, wherein the (B) condensation cure catalyst system is characterized by a molar ratio of (aza)carboxamidine / Co,Zn(alkyl)acetylacetonate of 15:0.15. Section 2. The (A) (hydrolyzable silyl group)-functional polyolefin prepolymer has the following limitations (i) to (iii): (i) each hydrolyzable silyl group independently has the formula (R 2 ) m (R 3 ) 3-m Si-, where subscript m is an integer 1, 2, or 3, and each R 2 is independently H, HO-, (C1-C6)alkoxy, (C2-C6)carboxy, phenoxy, (C1-C6)alkyl-phenoxy, ((C1-C6)alkyl)2N-, (C1-C6)alkyl(H)C=NO-, or ((C1-C6)alkyl)2C=NO-; 3 are independently (C1-C6) alkyl or phenyl; (ii) the polyolefin portion of (A) is a polyethylene-based, poly(ethylene-co-(C3-C 40 Item 1, characterized in that the moisture-curable polyolefin formulation is either (i) or (ii); or (ii) is an alpha-olefin based system, or a combination thereof; and (iii) is both (i) and (ii). Section 3. The moisture-curable polyolefin formulation according to item 1 or 2, wherein the mixture of the condensation curing catalyst system (B) is any one of (B1) to (B3): (B1) a blend of the (aza)carboxamidine and the Co,Zn(alkyl)acetylacetonate, (B2) a reaction product of the reaction of the (aza)carboxamidine and the Co,Zn(alkyl)acetylacetonate, and (B3) a combination of the (B2) reaction product and the (aza)carboxamidine and / or the Co,Zn(alkyl)acetylacetonate. Section 4. Item 4. The moisture-curable polyolefin formulation according to any one of items 1 to 3, wherein each (alkyl) acetylacetonate of the Co,Zn (alkyl) acetylacetonate is independently an unsubstituted acetylacetonate or a (C1-C6) alkyl substituted acetylacetonate. Section 5. Item 5. The moisture-curable polyolefin formulation according to any one of items 1 to 4, wherein the (aza)carboxamidine is an unsubstituted or substituted carboxamidine. Section 6. The carboxamidine is selected from the group consisting of (i) to (xix): (i) 1,8-diazabicyclo[5.4.0]undec-7-ene, (ii) 1,5-diazabicyclo[4.3.0]non-5-ene, (iii) 1,2,4-triazole-1-carboximidamide, (iv) acetamidine, (v) aminoacetamidine, (vi) benzamidine, (vii) 4-amino-benzamidine, (viii) 4-bromo-benzamidine, (ix) 4-chlorobenzamidine, (x) 4-fluoro ... amidine, (xi) 4-hydroxybenzamidine, (xii) 4-methoxybenzamidine, (xiii) 4-methylbenzamidine, (xiv) 4-trifluoromethylbenzamidine, (xv) N,N'-formamidine, (xvi) N,N'-diphenylformamidine, (xvii) pivalamidine, (xviii) 3-pyridine-3-carboxyimidamide, and (xix) cyclopropylamidine. Section 7. Item 5. The moisture-curable polyolefin formulation according to any one of items 1 to 4, wherein the (aza)carboxamidine is an unsubstituted or substituted guanidine. Section 8. Item 7, wherein the guanidine is any one of (i) to (viii): (i) 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, (iii) 1,1,3,3-tetramethylguanidine, (iv) 1,1,2,3,3-pentamethylguanidine, (v) 2-tert-butyl-1,1,3,3-tetramethylguanidine, (vi) 1,8-bis(tetramethylguanidino)naphthalene, (vii) 1-aminopyrazole, and (viii) 1H-pyrazole-1-carboxamide. The moisture-curable polyolefin formulation according to item 7. Section 9. Additives (C) to (L): (C) organic peroxide, (D) scorch retarder, (E) antioxidant, (F) tree retarder (water tree and / or electrical tree retarder), (G) colorant, (H) moisture scavenger, (I) hindered amine light stabilizer, (J) processing aid, (K) moisture generator, and (L) any combination of two or more of (C) to (K), The moisture-curable polyolefin formulation according to any one of items 1 to 8, further comprising at least one additive selected from the group consisting of (C) organic peroxide, (D) scorch retarder, (E) antioxidant, (F) tree retarder (water tree and / or electrical tree retarder), (G) colorant, (H) moisture scavenger, (I) hindered amine light stabilizer, (J) processing aid, (K) moisture generator, and (L) (C) to (K). Section 10. A method for preparing a moisture-curable polyolefin formulation, comprising: (A) mixing components including a (hydrolyzable silyl group)-functional polyolefin prepolymer and (B) a condensation curing catalyst system to obtain a mixture including (A) and (B); and melting or extruding the mixture to prepare the moisture-curable polyolefin formulation according to any one of items 1 to 9. Section 11. Item 10. A moisture-cured polyolefin product produced by moisture curing the moisture-curable polyolefin formulation according to any one of items 1 to 9, or the moisture-curable polyolefin formulation produced by the method according to item 10, to obtain a moisture-cured polyolefin product. Section 12. Item 12. A manufactured article comprising a shaped form of the moisture-curable polyolefin formulation according to any one of items 1 to 9, or the moisture-cured polyolefin product according to item 11. Section 13. Item 12. A coated conductor comprising a conductive core and a polymer layer at least partially surrounding the conductive core, wherein at least a portion of the polymer layer comprises the moisture-cured polyolefin product according to item 11. Section 14. 14. A method of conducting electricity, comprising applying a voltage across a conductive core of the coated conductor of claim 13 to generate a flow of electricity through the conductive core. Section 15. 1. A condensation cure catalyst system comprising: a mixture of DBU and Co(II)((alkyl)acac)2 having a molar ratio of DBU / Co(II)((alkyl)acac)2 of 1.5:1 to 2.4:1; a mixture of DBU and Co(III)((alkyl)acac)3 with a molar ratio of DBU / Co(III)((alkyl)acac)3 of 1:1 to 2:1; a mixture of TMG and Zn(II)((alkyl)acac)2 having a molar ratio of TMG / Zn(II)((alkyl)acac)2 of 1.5:1 to 2.4:1; a mixture of DBU and Zn(II)((alkyl)acac)2 having a DBU / Zn(II)((alkyl)acac)2 molar ratio of 0.19:1 to 10:1; and a mixture of DBN and Zn(II)((alkyl)acac)2 having a molar ratio of DBN / Zn(II)((alkyl)acac)2 of 1.5:1 to 2.4:1; A condensation cure catalyst system wherein DBN is 1,5-diazabicyclo[4.3.0]non-5-ene, DBU is 1,8-diazabicyclo[5.4.0]undec-7-ene, TMG is 1,1,3,3-tetramethylguanidine, and each (alkyl)acac is independently an unsubstituted acetylacetonate or a (C1-C6) alkyl substituted acetylacetonate having 1 to 5 unsubstituted (C1-C6) alkyl groups.
Claims
1. 1. A moisture curable polyolefin formulation comprising: (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer; (B) a condensation cure catalyst system comprising a mixture made by contacting at least one compound selected from the group consisting of 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 1,1,3,3-tetramethylguanidine (TMG) (collectively referred to as "(aza)carboxamidines") with a compound that is a zinc acetylacetonate coordination complex, wherein the acetylacetonate is unsubstituted or substituted with 1 to 5 alkyl groups, each alkyl group being unsubstituted (collectively referred to as "Zn(alkyl)acetylacetonates"), wherein the Zn(alkyl)acetylacetonates are zinc(II) ((alkyl)acetylacetonates). 2 is selected from the amount of (A) is 79.0 to 99.99 weight percent (wt%) and the amount of (B) is 21.0 to 0.01 wt% of the moisture-curable polyolefin formulation, The moisture-curable polyolefin formulation, wherein said (B) condensation cure catalyst system is characterized by a molar ratio of (aza)carboxamidine / Zn(alkyl)acetylacetonate of 15:1 to 0.15:
1.
2. The (A) (hydrolyzable silyl group)-functional polyolefin prepolymer satisfies limitations (i) to (iii): (i) each hydrolyzable silyl group independently represents a group of the formula (R 2 ) m (R 3 ) 3-m Si-, where subscript m is an integer of 1, 2, or 3, and each R 2 are independently H, HO-, (C 1 -C 6 ) alkoxy, (C 2 -C 6 ) carboxy, phenoxy, (C 1 -C 6 ) alkyl-phenoxy, ((C 1 -C 6 ) alkyl) 2 N-, (C 1 -C 6 ) alkyl(H)C=NO-, or ((C 1 -C 6 ) alkyl) 2 C=NO-, and each R 3 is independent, (C 1 -C 6 ) alkyl or phenyl; (ii) The polyolefin portion of (A) is a polyethylene-based, poly(ethylene-co-(C 3 -C 40 ) alpha-olefins), or combinations thereof; and (iii) both (i) and (ii); 2. The moisture-curable polyolefin formulation according to claim 1, characterized in that
3. The mixture of the condensation curing catalyst system (B) is the following (B1) to (B3): (B1) a blend of said (aza)carboxamidine and said Zn(alkyl)acetylacetonate; (B2) the reaction product of the reaction of said (aza)carboxamidine with said Zn(alkyl)acetylacetonate; (B3) a combination of the reaction product of (B2) with the (aza)carboxamidine and / or the Zn(alkyl)acetylacetonate; 3. The moisture-curable polyolefin formulation according to claim 1 or 2, which is any one of:
4. The acetylacetonate may be an unsubstituted acetylacetonate or (C 1 -C 6 4. The moisture-curable polyolefin formulation of claim 1, wherein the acetylacetonate is an alkyl substituted acetylacetonate.
5. The moisture curable polyolefin formulation of any one of claims 1 to 4, further comprising at least one additive selected from additives (C) to (L): (C) organic peroxides, (D) scorch retarders, (E) antioxidants, (F) tree retarders (water tree and / or electrical tree retarders), (G) colorants, (H) moisture scavengers, (I) hindered amine light stabilizers, (J) processing aids, (K) moisture generators, and (L) a combination of any two or more of (C) to (K).
6. A method of making a moisture-curable polyolefin formulation comprising: mixing components comprising (A) a (hydrolyzable silyl group)-functional polyolefin prepolymer and (B) a condensation cure catalyst system to obtain a mixture comprising (A) and (B); and melting or extruding the mixture to make the moisture-curable polyolefin formulation of any one of claims 1 to 5.
7. A moisture-cured polyolefin product, which is a moisture-cured product of the moisture-curable polyolefin formulation described in any one of claims 1 to 5.
8. An article of manufacture comprising a shaped form of the moisture-curable polyolefin formulation of any one of claims 1 to 5, or the moisture-cured polyolefin product of claim 7.
9. 10. A coated conductor comprising: a conductive core; and a polymeric layer at least partially surrounding the conductive core, at least a portion of the polymeric layer comprising the moisture-cured polyolefin product of claim 7.
10. 10. A method of conducting electricity comprising applying a voltage across a conductive core of the coated conductor of claim 9 to cause a flow of electricity through the conductive core.
Citation Information
Patent Citations
Silane cross-linked polyolefin insulation wire
JP2012256527A
Curable composition based on a silane group-containing polymer and a zinc catalyst
JP2016521787A
Curable organopolysiloxane composition
JP2017521538A
Curable coating compositions of silane functional polymers
US20160244606A1
Curable resin composition
WO2010128602A1