Optical diffraction element, optical computing device, and method for manufacturing optical diffraction element

The optical diffraction element with individually set refractive indices and uniform thickness in subcells, using a multi-block copolymer and guide, addresses the limitation of thickness-only setting, enhancing optical processing efficiency and reducing deformation.

JP7554900B2Active Publication Date: 2024-09-20FUJIKURA LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023500679
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-19
Filing Date
2022-01-27
Publication Date
2024-09-20
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing optical diffraction elements only individually set the thickness of microcells, but not the refractive index, limiting their optical processing capabilities.

Method used

An optical diffraction element with microcells composed of subcells, each having a specific refractive index and orientation, achieved through a multi-block copolymer with mesogenic groups and a guide for self-assembly, allowing individual setting of refractive indices and uniform thickness.

Benefits of technology

Enables higher optical processing efficiency by individually setting refractive indices, reducing deformation, and enhancing phase change capabilities of microcells, thus improving optical calculations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554900000005
    Figure 0007554900000005
  • Figure 0007554900000007
    Figure 0007554900000007
  • Figure 0007554900000008
    Figure 0007554900000008
Patent Text Reader

Abstract

In order to provide an optical diffractive element of a system for individually setting the refractive indices of a plurality of microcells, this optical diffractive element is provided with a plurality of microcells arranged along a specific plane, each of the plurality of microcells comprising a plurality of sub-cells. Each of the sub-cells is configured such that the refractive index with respect to at least one direction out of the in-plane directions of the specific plane will be any refractive index out of a prescribed number n (n being an integer 2 or greater) types of refractive indices.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical diffraction element including a plurality of microcells, an optical computing device including a plurality of such optical diffraction elements, and a method for manufacturing such an optical diffraction element. [Background technology]

[0002] There is known an optical diffraction element in which an optical diffraction structure is formed on one of the main surfaces of a substrate, the optical diffraction structure having a plurality of microcells each having a different thickness or refractive index, and optically executing a predetermined calculation by causing light transmitted through each microcell to interfere with each other. Here, the "microcell" refers to a cell having a cell size of less than 10 μm, for example. Also, the "cell size" refers to the square root of the cell area.

[0003] An optical arithmetic device using a plurality of optical diffraction elements has the advantage of being faster and consuming less power than an electrical arithmetic device using a processor. Patent Document 1 discloses an optical neural network having an input layer, an intermediate layer, and an output layer. The optical diffraction element described above can be used, for example, as the intermediate layer of such an optical neural network. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] U.S. Patent No. 7,847,225 Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, in the case of setting the thicknesses of a plurality of (here, 200×200) microcells A individually in an optical diffraction element, a configuration as shown in FIG. 15 can be adopted.

[0006] 15 includes a substrate 111 made of a light-transmitting layered member, and an optical diffraction structure 112. The optical diffraction structure 112 is composed of a plurality of microcells A formed on one main surface 1111 of the substrate 111. In the optical diffraction structure 112, the bottom surface of the microcells A is square. Therefore, the cell size of the optical diffraction structure 112 coincides with the length L of one side of the bottom surface.

[0007] In the optical diffraction structure 112, the thickness of the multiple microcells A is individually set to set the amount of phase change of each signal light LS passing through each microcell A. The optical diffraction structure 112 causes each signal light LS, the phase of which is changed according to the thickness of each microcell A, to interfere with each other. In this way, the optical diffraction element 112 optically executes a predetermined calculation. Note that in FIG. 15, the signal light LS is illustrated only for the microcell A shown in an enlarged view.

[0008] As described above, although optical diffraction elements in which the thicknesses of a plurality of microcells are set individually are known, optical diffraction elements in which the refractive indexes of a plurality of microcells are set individually are not known.

[0009] An object of the present invention is to provide an optical diffraction element in which the refractive indexes of a plurality of microcells are individually set. [Means for solving the problem]

[0010] In order to solve the above problems, an optical diffraction element according to one embodiment of the present invention comprises a plurality of microcells arranged along a specific plane, each of which includes a plurality of subcells, and each subcell has a refractive index in at least one of the in-plane directions of the specific plane that is one of n predetermined types of refractive indexes (n is an integer of 2 or more).

[0011] In order to solve the above problems, an optical computing device according to one embodiment of the present invention is configured to include N (N is an integer equal to or greater than 2) optical diffraction elements according to the above embodiment, and the areas in which the multiple microcells of each optical diffraction element are provided overlap.

[0012] In order to solve the above problems, a method for manufacturing an optical diffraction element according to one aspect of the present invention is a method for manufacturing an optical diffraction element including a plurality of microcells, each of which includes a plurality of subcells. In this manufacturing method, each subcell includes a multi-block copolymer in which a first segment formed of a block polymer containing a mesogen group having liquid crystal properties and a second segment formed of a block polymer not containing the mesogen group are alternately connected, and the total number of segments is at least two, and a guide for self-organizing the multi-block copolymer, and the method includes the steps of providing the guide on a main surface of a substrate and forming the multi-block copolymer so as to cover the guide, so that the orientation direction of the mesogen group in each subcell is one of n predetermined orientation directions. Effect of the Invention

[0013] According to one aspect of the present invention, it is possible to provide an optical diffraction element and an optical computing device that allow the refractive indexes of a plurality of microcells to be set individually. [Brief description of the drawings]

[0014] [Figure 1] 1A is a schematic diagram showing an arrangement of a plurality of microcells in an optical diffraction element according to a first embodiment of the present invention, and FIG. 1B is a schematic diagram showing a cross section of the optical diffraction element shown in FIG. [Diagram 2] 2 is a schematic diagram showing an arrangement of a plurality of subcells in each microcell of the optical diffraction element shown in FIG. 1. [Diagram 3] FIG. 3(a) is a schematic diagram of the subcell shown in FIG. 2. FIG. 3(b) is a schematic diagram showing a diblock copolymer contained in the subcell shown in FIG. [Figure 4] (a) is a structural formula of the diblock copolymer shown in (b) of Figure 3. (b) is a structural formula of the mesogen group contained in the first segment of the diblock copolymer shown in (a). [Diagram 5] 3(a) to (d) are schematic diagrams showing a first modified example of the subcell shown in FIG. 3(a). [Figure 6] 3(a) to (d) are schematic diagrams showing a second modified example of the subcell shown in FIG. 3(a). [Figure 7] 5 is a schematic diagram showing a cross section of an optical calculation device according to a second embodiment of the present invention. FIG. [Figure 8] FIG. 1(a) is a perspective view of a structure according to a first reference embodiment, FIG. 1(b) is a schematic diagram of an enlarged portion of the structure shown in FIG. 1(a), and FIG. 1(c) is a schematic diagram of two triblock copolymers contained in the structure shown in FIG. [Figure 9] (a) is the structural formula of the triblock copolymer shown in (b) and (c) of Figure 8. (b) is the structural formula of the dye shown in (b) and (c) of Figure 8. (c) is the structural formula of the cross-linking material shown in (b) and (c) of Figure 8. [Figure 10] FIG. 11 is a perspective view of an optical diffraction element according to a third embodiment of the present invention. [Figure 11] 11 is a perspective view of a microcell included in the optical diffraction element shown in FIG. [Figure 12] FIG. 2 is a schematic diagram of a gel according to a second embodiment of the present invention. [Figure 13] 10 is a flowchart of a manufacturing method according to a fourth embodiment of the present invention. [Figure 14] 14(a) to (e) are schematic diagrams of the gel or structure in each step included in the production method shown in FIG. [Figure 15] FIG. 1 is a perspective view showing a conventional optical diffraction element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [First embodiment] An optical diffraction element 10 according to a first embodiment of the present invention will be described with reference to FIGS. 1 to 5. FIG. 1(a) shows a plurality of microcells 11 in the optical diffraction element 10. ij FIG. 1(b) is a schematic diagram showing the arrangement of the microcells 11. Here, each of i and j is an integer satisfying 1≦i, j≦3. FIG. 1(b) is a schematic diagram showing the A-A′ cross section of the optical diffraction element 10 (see FIG. 1(a)). FIG. 2 is a schematic diagram showing the arrangement of the microcells 11. ij FIG. 3(a) is a schematic diagram showing the arrangement of a plurality of subcells in a semiconductor device. 31 FIG. 3(b) shows a schematic diagram of subcell 12. 31 Diblock copolymer 12P contained in 31 4 is a schematic diagram showing the structure of a diblock copolymer 12P (a) in FIG. 4. The structure of an example of a mesogen group contained in a segment S1 of the diblock copolymer (b) in FIG. 4 is a schematic diagram showing the structure of a diblock copolymer 12P (a) in FIG. 4. The structure of an example of a mesogen group contained in a segment S1 of the diblock copolymer (b).

[0016] 1, an orthogonal coordinate system is defined so that the principal surfaces of the substrates 101 and 102 constituting the optical diffraction element 10 are parallel to the xy plane, and the normal direction of the substrates 101 and 102 is the z-axis direction. ij The direction parallel to the rows and the direction parallel to the columns are defined as the x-axis and the y-axis, respectively. i ,LS o The propagation direction of the laser beam from the microcell 11 (see FIG. 1B) is defined as the positive direction of the z-axis. ij The directions in which the column numbers and row and column numbers increase are defined as the positive x-axis direction and the positive y-axis direction, respectively.

[0017] The coordinate system shown in FIGS. 2 and 3 is similar to the coordinate system shown in FIG.

[0018] <Outline of optical diffraction element> The optical diffraction element 10 includes microcells 11 ij By individually setting the refractive index of each microcell, ijThe optical diffraction element is configured to set the amount of phase change of each signal light passing through the optical diffraction element. The wavelength λ can be appropriately determined within a band of 360 nm or more and 1000 μm or less depending on the application, etc., during the design stage of the optical diffraction element. This band is composed of the visible range (360 nm or more and less than 830 nm), the near infrared range (830 nm or more and less than 2 μm), the mid infrared range (2 μm or more and less than 4 μm), and the far infrared range (4 μm or more and 1000 μm or less). In this embodiment, the signal light LS i ,LS o The wavelength λ is set to 400 nm. The wavelength λ may be at least a part of the wavelengths included in the band of 360 nm or more and 1000 μm or less.

[0019] In FIG. 1B, the signal light beams incident on the optical diffraction element 10 are collectively referred to as signal light LS i The signal light beams emitted from the optical diffraction element 10 are collectively referred to as signal light LS o It states that:

[0020] The signal light incident on the optical diffraction element 10 is guided to each microcell 11. ij When passing through each microcell, ij The phase of the light can be changed according to the refractive index of each microcell 11. ij Each signal light LS emitted from o Each signal light LS whose phase has been changed o In this way, the optical diffraction element 10 optically executes a predetermined operation.

[0021] <Configuration of optical diffraction element> As shown in FIG. 1B, the optical diffraction element 10 is made up of nine microcell groups 11 arranged in a matrix of three rows and three columns. 11 ~11 13 ,11 21 ~11 23 ,11 31 ~11 33In this embodiment, the optical diffraction element 10 includes a pair of substrates 101 and 102, a spacer 103, and a diblock copolymer 12P. The microcell group 11 is realized using the substrates 101 and 102, the spacer 103, and the diblock copolymer 12P.

[0022] (container) Substrate 101 is a layered member having a pair of main surfaces, 1011 and 1012. Substrate 102 is a layered member and has the same configuration as substrate 101. Substrate 102 also has a pair of main surfaces, 1021 and 1022. Substrates 101 and 102 are arranged such that main surfaces 1012 and 1021, which are adjacent main surfaces, face each other. In (b) of FIG. 1, substrate 101 is arranged on the negative side of the z axis, and substrate 102 is arranged on the positive side of the z axis.

[0023] In this embodiment, acrylic resin is used as the material for forming the substrates 101 and 102. However, the material for forming the substrates 101 and 102 is a material that is suitable for the optical transmission of the signal light LS with λ=400 nm. i ,LS o The material constituting the substrates 101 and 102 is not limited to resins such as acrylic resins, as long as the material has light-transmitting properties. The material constituting the substrates 101 and 102 may be a glass material such as quartz glass.

[0024] The main surface 1011 is a surface that reflects the signal light LS to the optical diffraction element 10. i The principal surface 1022 constitutes an incident surface onto which the signal light LS is incident from the optical diffraction element 10. o This forms the main slope from which the light is emitted.

[0025] A spacer 103 having a predetermined thickness is provided between the substrate 101 and the substrate 102. The thickness of the spacer 103 defines the distance between the substrate 101 and the substrate 102 which face each other.

[0026] The substrates 101 and 102 and the spacer 103 are joined together to form a sealed space (see FIG. 1(b)). This sealed space is filled with a diblock copolymer 12P. Thus, the substrates 101 and 102 and the spacer 103 form a container that contains the diblock copolymer 12P. The diblock copolymer 12P will be described later with reference to FIGS. 3 and 4.

[0027] (Guide and Diblock Copolymer) Although not shown in FIG. 1B, a guide 12g is provided on a main surface 1012, which is one of the pair of main surfaces of the substrate 101 and is the main surface with which the diblock copolymer 12P is in contact. The guide 12g is made of a material that is transparent to light with a wavelength λ. The guide 12g can be patterned into a desired pattern by curing a photoresist using, for example, electron beam lithography.

[0028] The thickness of the guide 12g may be equal to or smaller than the thickness of the spacer 103. As described later, the diblock copolymer 12P is oriented by self-organization triggered by the guide 12g. Therefore, even if the thickness of the guide 12g is smaller than the thickness of the spacer 103, substantially all of the diblock copolymer 12P can be self-organized.

[0029] The diblock copolymer 12P contains a mesogen group MG having liquid crystallinity. The mesogen group MG is aligned along either the x-axis direction or the y-axis direction according to the shape of the guide 12g. The structure of the diblock copolymer 12P and the alignment of the mesogen group MG will be described later with reference to FIG. 2.

[0030] In the optical diffraction element 10, as shown in FIG. 1A, an effective area through which the signal light passes is divided into 3 rows and 3 columns (i.e., 9 areas), and each area is called a microcell 11. ij In FIG. 1(b), a microcell 11 ij Of these, the second row microcell is Microcell 11.21 ~11 23 Also, each microcell 11 ij Each area is divided into 4 rows and 4 columns (i.e. 16 areas) and each area is subcell 12 kl Here, k and l are integers satisfying 1≦k, l≦4. kl are collectively referred to as a subcell group 12.

[0031] Therefore, in the optical diffraction element 10, each microcell 11 ij The microcells 11 are arranged in a matrix along a main surface 1012, which is an example of a specific plane. ij 12 kl Includes.

[0032] Here, the term "microcell" refers to a cell with a cell size of less than 10 μm, for example. Also, the term "cell size" refers to the square root of the area of ​​the cell. For example, when the shape of the microcell in plan view is a square, the cell size is the length of one side of the cell. The lower limit of the cell size is not particularly limited, but is, for example, 1 nm.

[0033] In this embodiment, each microcell 11 ij The thickness of each microcell 11 ij Each subcell 12 kl The thickness of each microcell 11 is determined by the distance between the substrate 101 and the substrate 102 (i.e., the thickness of the spacer 103). ij The thickness of each subcell 12 kl The thicknesses are approximately equal.

[0034] The guide 12g is arranged on each of the sub-cells 12, each of which is square in shape when the main surface 1012 is viewed in a plan view along the z-axis direction. kl The subcells 12 are arranged in a lattice pattern so as to separate the subcells 12 from each other (see FIG. 2). kl In FIG. 3(a), a notch g is provided in a portion of the guide 12g surrounding the subcell 12. kl As an example of subcell 1231 The notch g and the alignment direction of the mesogen group MG will be described using the following formula. kl The length L of one side of the signal light L is set to 100 nm. However, the length L is not limited to this. i ,L o The wavelength λ (400 nm in this embodiment) of each microcell 11 ij The refractive index may be determined according to the number of gradations in the refractive index.

[0035] Each microcell 11 ij In order to increase the amount of phase change that occurs when light passes through each microcell 11, ij The length of one side of each microcell 11 is preferably λ or less, and more preferably λ / 2 or less. ij The length of one side is set to 200 nm, which is λ / 2.

[0036] In this embodiment, each microcell 11 ij 16 subcells 12 kl According to this configuration, each microcell 11 ij The number of gradations is 17. When such a configuration is adopted, L=50 nm may be adopted. ij In the case where the microcell 11 is divided into a subcell group 12 of N rows and N columns (N is an integer of 2 or more), ij The number of gradations is N 2 It becomes +1 gradation.

[0037] Subcell 12 31 Prescriptive Guide 12g 31 The subcell 12 has two notches g. These two notches g are both provided near the midpoints of the sides parallel to the x-axis direction. 31 The length of each side of is length L, and the length of the notch g is length L g In this case, the guide 12g parallel to the y-axis 31 The length of the guide 12g is 2L and is parallel to the x-axis direction. 31The length of is 2(LL g ) Therefore, subcell 12 31 In this case, the guide 12g is parallel to the y-axis direction. 31 The length of the guide 12g is parallel to the x-axis direction. 31 exceeds the length of

[0038] In this way, each subcell 12 kl In this case, the guide 12g is parallel to the x-axis direction. 31 The length of the guide 12g parallel to the y-axis direction 31 A notch g is provided on at least one of the four sides so that the length of the side is different from that of the side.

[0039] As described above, the diblock copolymer 12P is filled in the container formed by the substrates 101, 102 and the spacer 103. Therefore, as shown in FIG. 3(a), each subcell 12 kl (In FIG. 3(a), subcell 12 31 Inside is a diblock copolymer 12P kl (In FIG. 3(a), the diblock copolymer 12P 31 ) is filled. In the following, the diblock copolymer 12P 31 Take the diblock copolymer 12P as an example. kl In addition, each subcell 12 kl When it is not necessary to distinguish which subcell a particular block copolymer belongs to, the block copolymer is simply referred to as diblock copolymer 12P.

[0040] As shown in FIG. 3(b) and FIG. 4(a), the diblock copolymer 12P 31 The diblock copolymer 12P represented by the above is a diblock copolymer in which the segment S1 and the segment S2 are connected and the total number of segments is 2. However, the diblock copolymer 12P may be a multiblock copolymer in which the segment S1 and the segment S2 are alternately connected and the total number of segments is 3 or more.

[0041] The segments S1 and S2 are examples of the first and second segments, respectively. The block polymer constituting the segment S1 contains a mesogen group MG having liquid crystallinity (see (a) and (b) of FIG. 4). The mesogen groups MG shown in (b) of FIG. 4 are, in order from the top, 5CB (4'-pentyl-4-cyanobiphenyl), 4'-hexoxy-4-cyanobiphenyl, 4-butoxyphenylbenzoate, and 4-pentanoylphenylbenzoate.

[0042] Each of the mesogen groups MG contains two benzene rings connected in a straight chain. In this embodiment, the side chain direction in which the benzene rings of the mesogen group MG are connected in a straight chain is substantially perpendicular to the main chain direction in which the main chains of the segments S1 and S2 are extended. In FIG. 3(b), this side chain direction is indicated by an arrow D1.

[0043] However, the angle between the main chain direction and the side chain direction in the diblock copolymer 12P is not limited. On the other hand, the block polymer constituting the segment S2 does not contain a mesogen group MG.

[0044] The mesogenic group MG, which contains two benzene rings connected in a linear chain, has anisotropic refractive index. Specifically, it exhibits a high refractive index for linearly polarized light whose polarization direction is parallel to the direction of the side chains in which the benzene rings are connected in a linear fashion, and exhibits a low refractive index for linearly polarized light whose polarization direction is parallel to the direction perpendicular to the side chain direction. In FIG. 3(b), an ellipse is used as the shape representing the mesogenic group MG. In the ellipse representing the mesogenic group MG, the long axis direction corresponds to the polarization direction that exhibits a high refractive index, and the short axis direction corresponds to the polarization direction that exhibits a low refractive index.

[0045] In this embodiment, the block polymer constituting the segment S1 is hydrophilic, and the block polymer constituting the segment S2 is hydrophobic. Moreover, the surface of the above-mentioned guide 12g is treated to have hydrophobicity.

[0046] Therefore, the segment S2 made of a hydrophobic block polymer is 31 The segment S1, which is made of a hydrophilic block polymer, tends to aggregate in the vicinity of the guide 12g. 31 As a result, the diblock copolymer 12P 31 There is a force that tends to self-organize by arranging.

[0047] However, the polarity of the segment S1, the polarity of the segment S2, and the polarity of the guide 12g are not limited to the above combination. In the optical diffraction element 10, the surface of the guide 12g has either hydrophobic or hydrophilic polarity, and if one of the segments S1 and S2 is hydrophobic and the other is hydrophilic, the diblock copolymer 12P can be self-assembled.

[0048] As mentioned above, subcell 12 31 In this case, the guide 12g is parallel to the y-axis direction. 31 The length of the guide 12g is parallel to the x-axis direction. 31 Therefore, the length of the segment S2 is longer than the length of the guide 12g. 31 As a result, the particles aggregate in the portion of subcell 12 that is parallel to the y-axis direction. 31 In the present invention, the diblock copolymer 12P is used as shown in (a) and (b) of FIG. 31 In FIG. 3(a), the subcell 12 31 Only the right half region R of the subcell 12 is shown in an enlarged manner in FIG. 31 Similarly, the left half of the region is filled with diblock copolymer 12P 31 is oriented.

[0049] As a result, subcell 12 31 The polarization direction is diblock copolymer 12P 31 It exhibits a high refractive index when linearly polarized light is incident parallel to the side chain direction (the direction of arrow D1).

[0050] Microcell 11 shown in Figure 2 ij In subcell 12 31 In addition, subcell 12 14 ,12 21 ,12 23 ,12 24 ,12 32 ,12 34 ,12 41 is configured such that the length of the guide 12g parallel to the y-axis direction is greater than the length of the guide 12g parallel to the x-axis direction. Therefore, in these eight subcells, the side chain direction is approximately parallel to the arrow D1, and a high refractive index is exhibited when linearly polarized light parallel to the direction of the arrow D1 is incident.

[0051] Meanwhile, Microcell 11 ij In subcell 12 11 ,12 12 ,12 13 ,12 22 ,12 33 ,12 42 ,12 43 ,12 44 is configured such that the length of the guide 12g parallel to the x-axis direction is greater than the length of the guide 12g parallel to the y-axis direction. Therefore, in these eight subcells, the side chain direction is approximately parallel to the arrow D0 perpendicular to the arrow D1, and a low refractive index is exhibited when linearly polarized light parallel to the direction of the arrow D1 is incident.

[0052] As above, each of the 16 subcells 12 kl For linearly polarized light having a predetermined polarization direction (for example, a direction parallel to the arrow D1), the subcell 12 can take either a state "1" in which the refractive index is high or a state "0" in which the refractive index is low. kl The alignment direction of the mesogen group MG in each subcell 12 is one of two predetermined alignment directions (the direction of the arrow D0 and the direction of the arrow D1). kl The refractive index of each microcell 11 is one of two types in one of the in-plane directions of the xy plane (for example, the direction of the arrow D1). ij can express 17 gradations from 0 to 16 inclusive.

[0053] In addition, each microcell 11 ij The signal light passing through the microcell 11 is affected by the average refractive index over a size area of ​​approximately the same size as the wavelength λ (=400 nm). ij The refractive index of each of the 16 subcells 12 kl The refractive index is the average value of the refractive indexes.

[0054] When 5CB (4-Cyano-4'-pentylbiphenyl) shown in the top row of FIG. 4(b) is used as the mesogen group MG, the difference Δ between the refractive index for linearly polarized light whose polarization direction is parallel to the arrow D1 and the refractive index for linearly polarized light whose polarization direction is perpendicular to the arrow D1 is about 0.2 (example when λ=550 nm). Therefore, the maximum gradation value of 17 levels in microcell 11 is 100%. ij In the case where it is assumed that the phase of the signal light is delayed by one wavelength (400 nm in this embodiment) in each microcell 11, ij (i.e., each subcell 12 kl In addition, considering that the mesogen group MG is bonded only to the segment S1 of the segments S1 and S2 constituting the diblock copolymer 12P, each microcell 11 ij (i.e., each subcell 12 kl ) is preferably 6 μm or more in thickness.

[0055] (Manufacturing method) A brief description will now be given of a method for manufacturing the optical diffraction element 10 shown in Figures 1 and 2. This manufacturing method includes a step of providing a guide 12g and a step of filling with the diblock copolymer 12P.

[0056] The step of providing the guide 12g includes the steps of: klThis is a step of providing guides 12g on the main surface 1012 of the substrate 101 constituting a specific plane so that the alignment direction of the mesogen group MG in the substrate 101 is one of n predetermined alignment directions. Fig. 2 shows an example of the guides 12g provided on the main surface 1012. As described above, the guides 12g can be patterned into a desired pattern by curing a photoresist using, for example, electron beam lithography.

[0057] Next, a layer of the diblock copolymer 12P is formed so as to cover the main surface 1012 and the guide 12g. The method for forming the layer of the diblock copolymer 12P is not particularly limited, but for example, a solution of the diblock copolymer dissolved in a solvent can be formed into a uniform layer using a simple method such as spin coating or spray coating. By carrying out this step, the main surface 1012 on which the guide 12g is provided is covered with the diblock copolymer 12P. As a result, each of the subcells 12 kl The diblock copolymer 12P constituting the subcell 12, which includes the mesogen group MG, is self-assembled by the guide 12g. kl The alignment direction of the mesogenic group MG in the liquid crystal layer 100 takes any one of n predetermined alignment directions.

[0058] Next, a cavity can be formed between the substrates 101 and 102 by sandwiching a spacer 103 between the substrates 101 and 102. At this time, the orientation of the substrate 101 is determined so that the main surface 1012 on which the guides 12g are provided is on the cavity side. The spacer 103 can also be used as an alignment mark.

[0059] It is preferable that the spacer 103 has a uniform thickness. When the spacer 103 has a uniform thickness, the distance between the substrate 101 and the substrate 102 can be made uniform.

[0060] Furthermore, if no gap is required between the substrate 101 and the substrate 102, the spacer 103 can be omitted. In this case, the substrate 101, the spacer 103, and the substrate 102 may be laminated such that the spacer 103 is directly interposed between the substrate 101 and the substrate 102.

[0061] <Modification of subcell> In the above-described optical diffraction element 10, as shown in FIG. kl may be configured so that the orientation direction of the mesogenic group MG is one of two predetermined orientation directions (the direction of arrow D0 and the direction of arrow D1), i.e., the refractive index in one of the in-plane directions of the xy plane (for example, the direction of arrow D1) is one of n predetermined refractive indices.

[0062] FIG. 5(a) to (d) show subcell 12. kl FIG. 1 is a schematic diagram showing a first modified example of the subcell 12. kl is configured so that the orientation direction of the mesogenic group MG takes one of four predetermined orientation directions (the directions of arrows D0, D1, D2, D3), i.e., so that the refractive index in one of the in-plane directions of the xy plane (for example, the polarization direction Lp) takes one of four predetermined refractive indices.

[0063] In this modification, each subcell 12 kl The above configuration is realized by selecting the direction of the subcell 12 shown in FIG. 5(a) to (d). kl The state of the subcell 12 shown in FIG. 31 In addition, the state of the subcell 12 shown in (b) to (d) of FIG. kl The state of the subcell 12 shown in FIG. 31 The alignment direction of the mesogen group MG is obtained by rotating the liquid crystal display by 30 degrees each time. The arrows shown in (a) to (d) of Fig. 5 indicate the alignment direction of the mesogen group MG.

[0064] In addition, each subcell 12kl As shown in (a) to (d) of FIG. 6, the guide 12g has a lattice shape. kl Instead of the pin or dot guide 12g kl For example, as described in A. Tavakkoli KG et. al., "Templating Three-Dimensional Self-Assembled Structures in Bilayer Block Copolymer Films", Science 08 Jun 2012, Vol. 336, Issue 6086, pp. 1294-1298, a pin-shaped or dot-shaped guide 12g may be used to align the mesogen group MG. kl By arranging them in a matrix, the mesogen groups MG can be aligned. kl The outline of the slit is shown by a two-dot chain line.

[0065] In the state shown in FIG. 6(a), the guide 12g kl The subcell 12 shown in (b) to (d) of FIG. 6 is configured so that the side chain direction of the mesogen group MG is parallel to the polarization direction Lp. kl The state of the subcell 12 shown in FIG. kl 6(a) to 6(d) show the alignment directions of the mesogen groups MG.

[0066] In addition, in (b) and (c) of FIG. 6, the guides 12g arranged in a matrix kl In order to clearly show that the row and column directions of the subcell 12 are rotated, the row and column directions of the subcell 12 are square. kl The outline of the guide 12g (two-dot chain line) is also rotated. kl If we adopt the dotted line, subcell 12 kl The contour is not rotated, guide 12g klThe row and column directions of each subcell 12 can also be rotated. kl That is, each of the subcells 12 can be arranged in close contact with each other. kl This eliminates gaps that may occur in the

[0067] According to this configuration, the microcell 11 ij This increases the number of possible gradations.

[0068] Second Embodiment An optical arithmetic device 1 according to a second embodiment of the present invention will be described with reference to Fig. 7. Fig. 7 is a schematic diagram showing a cross section of the optical arithmetic device 1. As shown in Fig. 7, the optical arithmetic device 1 includes three optical diffraction elements 10a, 10b, and 10c. The optical diffraction elements 10a, 10b, and 10c are configured in the same manner as the optical diffraction element 10 shown in Fig. 1, and the reference characters have a, b, and c suffixed thereto to distinguish them from one another.

[0069] In the optical calculation device 1, the optical diffraction elements 10c, 10b, and 10a each include a plurality of microcells 11 ij 7, the optical diffraction elements 10c, 10b, and 10a are stacked in this order with the regions where the microcells 11 are provided overlapping each other. ij Of these, Microcell 11 21 ,11 22 ,11 23 Only the above is shown.

[0070] The substrate 102a of the optical diffraction element 10a and the substrate 101b of the optical diffraction element 10b are fixed to each other. The substrate 102b of the optical diffraction element 10b and the substrate 101c of the optical diffraction element 10c are fixed to each other.

[0071] Each of the optical diffraction elements 10a, 10b, and 10c optically executes a predetermined operation. i The signal light LS represents the result of performing predetermined operations in sequence on o Output.

[0072] In this embodiment, the number N (N is an integer of 2 or more) of the optical diffraction elements 10a, 10b, and 10c included in the optical calculation device 1 is 3. However, N is not limited to 3 and can be appropriately determined depending on the purpose of the calculation, etc.

[0073] [First reference form] A structure 20 according to a first embodiment of the present invention will be described with reference to Fig. 8 and Fig. 9. Fig. 8(a) is a perspective view of the structure 20, Fig. 8(b) is a schematic diagram of an enlarged portion of the structure 20, and Fig. 8(c) is a schematic diagram of two triblock copolymers 21 contained in the structure 20. Fig. 9(a) is a structural formula of a specific example of the triblock copolymer 21, Fig. 9(b) is a structural formula of a specific example of the dye 22 contained in the structure 20, and Fig. 9(c) is a structural formula of a specific example of the cross-linking agent 23 contained in the structure 20.

[0074] <Structure> In this embodiment, the shape of the structure 20 is a cube (see FIG. 8(a)). However, the shape of the structure 20 is not limited to this. The shape of the structure 20 can be appropriately determined according to the pattern of exposure performed in the exposure process (see FIG. 12 and FIG. 13(b)) included in the manufacturing method described later in the fifth embodiment. Furthermore, the structure 20 is not limited to a three-dimensional structure as shown in FIG. 8(a) and may be a two-dimensional structure.

[0075] In the structure 20 of this embodiment, 500 nm is adopted as the length L of one side. Therefore, the structure 20 has a nanostructure, which is a nanometer-scale structure. However, the structure of the structure 20 is not limited to a nanostructure, and may be a microstructure, which is a microscale structure. However, when manufacturing a structure using the existing ImpFab method, the smaller the size of the structure, the more likely it is that the shape will be distorted due to shrinkage that occurs in the dehydration and sintering process. Therefore, the effect obtained by the structure 20 and the manufacturing method M20 described later (see Figs. 13 and 14) becomes more prominent as the size of the structure 20 becomes smaller. Specifically, the structure 20 and the manufacturing method M20 can be suitably used when the minimum width of the pattern is less than 10 μm, and can be more suitably used when the minimum width of the pattern is less than 1 μm. Note that the nanometer-scale structure refers to a structure in which the minimum width of the pattern is less than 1 μm, and the micrometer-scale structure refers to a structure in which the minimum width of the pattern is less than 1 mm.

[0076] The structure 20 contains a triblock copolymer 21, a dye 22, and a cross-linking agent 23 (see FIG. 8(b)). In FIG. 8(c), two triblock copolymers 21 contained in the structure 20 are enlarged and diagrammatically illustrated.

[0077] (Triblock copolymer) Triblock copolymer 21, which is an example of a multiblock copolymer, is composed of hydrophobic segments 211 and hydrophilic segments 212 bonded alternately (see FIG. 8(c)). Segment 211 is an example of a first segment, and segment 212 is an example of a second segment.

[0078] In this embodiment, each of the segment 211 and the segment 212 is composed of one block polymer. However, the block polymer constituting the segment 211 has hydrophobic properties, and the block polymer constituting the segment 212 has hydrophilic properties. An example of the segment 211 and the segment 212 will be described later with reference to (a) of FIG. However, the segment 211 may be composed of a plurality of block polymers having hydrophobic properties, and the segment 212 may be composed of a plurality of block polymers having hydrophilic properties.

[0079] In the present embodiment, the triblock copolymer 21 has the segment 211, the segment 212, and the segment 211 bonded in this order. In other words, the triblock copolymer 21 is composed of two segments 211 and the segment 212 interposed between these two segments 211. Therefore, the total number of segments in the triblock copolymer 21 is 3. However, the total number of segments is not limited to 3 and can be appropriately determined as long as it is 3 or more. In this way, the structure 20 may be a multi-block copolymer instead of a triblock copolymer. The total number of segments is preferably an odd number, and more preferably 3.

[0080] In the manufacturing method M20 described later, a polymer gel (hydrogel in the manufacturing method M20) obtained by swelling the triblock copolymer 21 in a solvent (water in the manufacturing method M20) is used as an intermediate for manufacturing the structure 20 (hereinafter, also referred to as a gel for manufacturing a microstructure). Since the total number of segments is an odd number, block polymers having the same polarity are located at both ends of the triblock copolymer 21. Therefore, when forming a polymer gel, the ends of the multiple triblock copolymers 21 can be easily aggregated together. In addition, since the total number of segments is 3, it is possible to prevent the portions other than the ends of the multiple triblock copolymers 21 from aggregating. Therefore, it is easy to make the pitch of the polymer matrix constituting the polymer gel uniform.

[0081] In the present embodiment, the triblock copolymer 21 is designed on the assumption that water, which is an example of a hydrophilic solvent, is used as the solvent when preparing the gel for producing a microstructure. Therefore, a triblock copolymer having segments 211 at both ends is used as the triblock copolymer 21. However, when a hydrophobic solvent is used when preparing the gel for producing a microstructure, a triblock copolymer having segments 212 at both ends may be used as the triblock copolymer 21.

[0082] (Pigments and crosslinking agents) 8(b) and 8(c), in at least one of the plurality of triblock copolymers 21, a dye 22 is bonded to a segment 212 interposed between two segments 211 at both ends. In addition, the dyes 22 are crosslinked to each other by a crosslinking agent 23. Therefore, at least some of the plurality of triblock copolymers 21 are crosslinked to each other via the dye 22.

[0083] When a triblock copolymer having segments 212 at both ends is used as the triblock copolymer 21 , the dye 22 may be bonded to the segment 211 interposed between the two segments 212 .

[0084] (Specific examples of block polymers, dyes, and crosslinkers) Examples of block polymers constituting the segments 211 and 212 constituting the triblock copolymer 21 include poly(butyl methacrylate) (PBMA) and poly(methacrylic acid) (PMMA), respectively. In the specific example shown in (a) of Figure 9, the degree of polymerization n of the left-hand segment 211 is n = 134, the degree of polymerization m of the segment 212 is m = 273, and the degree of polymerization k of the right-hand segment 211 is k = 192.

[0085] However, the block polymers constituting the segments 211 and 212 are not limited to PBMA and PMMA, respectively. As other block polymers constituting the segment 211, methacrylates and acrylates having an alkyl chain, such as poly(hexyl methacrylate) and poly(octyl methacrylate), are preferably used, but are not limited thereto, and polymers having a hydrophobic side chain, such as an alicyclic functional group or an alkyl fluoride, can be preferably used. As other block polymers constituting the segment 212, methacrylates and acrylates having a carboxylic acid group, such as poly(acrylic acid), are preferably used, but are not limited thereto, and can be polymers containing a functional group that can react with a desired dye.

[0086] The segment 212 to which the dye 22 is bonded has a number average molecular weight (M n ) and polystyrene equivalent weight average molecular weight (M W ) ratio (M W / M n) is preferably 3 or less, more preferably 2 or less, and most preferably 1.2 or less. The narrower the molecular weight distribution, the narrower the chain length distribution of the block polymer, and therefore the more uniform the hydrogel with the knit structure can be formed.

[0087] The molecular weight distribution of the segment 212 may be appropriately determined depending on the minimum width of the pattern in the microstructure or nanostructure of the structure 20 to be manufactured. The smaller the minimum width of the pattern, the smaller the molecular weight distribution of the segment 212 is preferably. Like the segment 212, the molecular weight distribution of the segment 211 is also preferably small. The segment 211 and the segment 212 can be manufactured using a precision polymerization method such as living radical polymerization, and therefore the molecular weight distribution can be made small.

[0088] Moreover, the ratio of block components in the segment 212 is preferably 80% or more and 100% or less, and more preferably 90% or more, when measured by 13C-NMR. The ratio of block components can be calculated from the sequence information of the triad in the 13C-NMR measurement. Here, the ratio of block components is defined as follows. (Ratio of block components) = (fractions that are all the same unit) / (total fractions) x 100 (%)

[0089] In addition, even if a block polymer is composed of multiple monomers, it will be counted in the above formula as long as all the triad components are the same. For example, in the case of a block copolymer composed of two types of monomers, A and B, it will be counted as an "AAA" fraction and a "BBB" fraction molecule, but other fractions containing different units such as "BAB" and "ABA" will not be counted in the above formula. By having the proportion of block components be 80% or more, it is possible to construct a gel with a more controlled structure and a knitted structure.

[0090] An example of the dye 22 is fluorescein, which is a fluorescent dye, or fluorescein in which the carboxyl group is replaced with a substituent R (see FIG. 9(b)). A cross-linking agent 23, which will be described later, is used as the substituent R. When the triblock copolymers 21 are not cross-linked to each other, as in a modified example of the structure 20, which will be described later, an amino group (NH2), a thiol group (SH), biotin, or the like can be used as the substituent R.

[0091] The cross-linking agent 23 is a cross-linking agent for aqueous resins, and an example thereof is 1,11-diazide-3,6,9-trioxaundecane, which is a diazide having a water-soluble skeleton (see FIG. 9(c)). When diazides or the like are used as cross-linking agents in a cross-linking reaction, it is preferable that the substituent introduced into the dye 22 is a functional group having an unsaturated double bond or triple bond.

[0092] <Optical diffraction element> An optical diffraction element 20A according to a third embodiment of the present invention will be described with reference to Fig. 10 and Fig. 11. Fig. 10 is a perspective view of the optical diffraction element 20A. Fig. 11 is a perspective view of a microcell 202 included in the optical diffraction element 20A. The optical diffraction element 20A can be said to be a modified example of the structure 20 shown in Fig. 8.

[0093] The optical diffraction element 20A has a nanostructure, similar to the structure 20. Also, similar to the structure 20, the optical diffraction element 20A contains a triblock copolymer in which the hydrophobic first segments 211 and the hydrophilic second segments 212 are alternately bonded, and the total number of segments is three.

[0094] (Microcell) However, the triblock copolymer contained in the optical diffraction element 20A differs from the triblock copolymer 21 contained in the structure 20 (FIGS. 8(b) and (c)) in that nanoparticles are bonded to the dye 22 instead of the cross-linking agent 23. In this modification, a microcell 202 containing nanoparticles will be described. The microcell 202 is a part of the triblock copolymer and is a region in which diamond nanoparticles are bonded to the dye 22.

[0095] As described above, in the triblock copolymer contained in the optical diffraction element 20A, one of the segments 211 and 212, that is, the segment 212 interposed between the two segments 211 at both ends, has a dye 22 and nanoparticles bonded to it in this order.

[0096] The nanoparticles are configured so that the refractive index is greater than the refractive index of the polymer matrix including the segments 211 and 212. In this modification, diamond nanoparticles are used as the nanoparticles. However, the material constituting the nanoparticles is not limited to diamond, and may be gold, silver, copper, or platinum, or may be carbon nanotubes, fullerene, titanium oxide, or silica. In addition, it is not necessary to use these materials alone, and they may be blends or alloys of these materials.

[0097] As a result, the refractive index of the region of the triblock copolymer where the dye 22 and the nanoparticles are bonded to the segment 212 is higher than the refractive index of the region where the dye 22 and the nanoparticles are not bonded to the segment 212. Hereinafter, the region where the dye 22 and the nanoparticles are not bonded to the segment 212 is referred to as a low refractive index section 201, and the region where the refractive index is higher than that of the low refractive index section 201 due to the nanoparticles is referred to as a microcell 202.

[0098] The refractive index of the triblock copolymer 21 constituting the low refractive index portion 201 is, for example, 1.4.

[0099] Meanwhile, the refractive index of diamond, which is used as the nanoparticle material, is 2.42. The refractive index of the microcell 202 depends on the density of the nanoparticles in the microcell 202. The density of the nanoparticles depends on the density of the dye 22 bound to the segment 212 and the particle size of the nanoparticles bound to the dye 22. The higher the density of the dye 22 bound to the segment 212, the more nanoparticles the microcell 202 can contain. Also, the larger the particle size of the nanoparticles, the more the volume per nanoparticle can be increased. As will be described later with reference to FIG. 11, in the microcell 202, the subcells 202 11 ,202 12 ,202 21 ,202 22 When the refractive index is to be different for each layer, the refractive index can be controlled by controlling the density of the dye 22. The density of the dye 22 can be controlled by the amount of exposure in the exposure step S13 shown in Figures 13 and 14. The higher the amount of exposure in the exposure step S13, the higher the density of the dye 22.

[0100] Therefore, the refractive index of the microcell 202 can be appropriately set within a range of 1 or more and less than 2.42. In other words, in the optical diffraction element 20A, the refractive index difference Δ between the low refractive index portion 201 and the microcell 202 can be appropriately set within a range of 0≦Δ≦1.02.

[0101] 15, the refractive index of the resin constituting the microcell A is 1.5, and therefore the refractive index difference with the air (refractive index 1) surrounding the periphery of the microcell A is approximately 0.5. Therefore, compared to the optical diffraction element 110, the optical diffraction element 20A can have a thinner microcell 202.

[0102] In this embodiment, the shape of the low refractive index portion 201 is a rectangular parallelepiped block. The size of the low refractive index portion 201 is such that the length of each side of a pair of bottom walls is 4.5 μm, and the thickness is 1.5 μm.

[0103] In this embodiment, each microcell 202 has a shape of a columnar pillar. The size of each microcell 202 is such that the length L of each side of a pair of bottom surfaces is 500 nm, and the thickness is 550 nm. The microcells 202 are embedded in the low refractive index portion 201 along the main surface of the low refractive index portion 201 in a matrix shape of 4 rows and 4 columns. The main surface of the low refractive index portion 201 is an example of a specific plane. Note that in FIG. 10, only one microcell 202 out of the 16 microcells 202 is labeled with a reference symbol.

[0104] (Subcell) As shown in FIG. 11, each microcell 202 is made up of four subcells 202 arranged in two rows and two columns. 11 ,202 12 ,202 21 ,202 22 However, the number of sub-cells constituting each microcell 202 is not limited to four, and can be determined appropriately according to the desired number of gradations.

[0105] Each subcell 202 11 ,202 12 ,202 21 ,202 22 The subcells 202 are configured to have one of two predetermined refractive indices, 1.4 and 2.42. In this embodiment, the refractive index is controlled according to the density of the nanoparticles. 11 ,202 12 ,202 21 ,202 22 The refractive index of isotropic is 1.4 or 2.42 in all directions. The number of gradations of the microcell 202 thus configured is 5.

[0106] In addition, each subcell 202 11 ,202 12 ,202 21 ,202 22 The types of predetermined refractive indexes that can be taken are not limited to two types and can be appropriately selected from a plurality of types.

[0107] The shapes and sizes of the low refractive index portion 201 and the microcell 202 are not limited to this modification, and can be determined as appropriate. The microcell 202 may be embedded inside the low refractive index portion 201 as shown in FIG. 10, or may be exposed from a pair of main surfaces of the low refractive index portion 201. When the microcell 202 is exposed on the main surfaces of the low refractive index portion 201, the thickness of the microcell 202 is equal to the thickness of the low refractive index portion 201.

[0108] <Optical computing device> 10, in the optical diffraction element 20A, a plurality of microcells 202 arranged in a matrix are embedded in a single layer in the low refractive index portion 201. However, in one aspect of the present invention, a configuration in which a plurality of microcells 202 arranged in a matrix are embedded in each of a plurality of layers in the low refractive index portion 201 may also be employed. In this case, the regions in which the plurality of microcells 202 are provided in each layer overlap each other.

[0109] According to this configuration, it is possible to realize an optical arithmetic device similar to the optical arithmetic device shown in Fig. 7 by using a configuration in which a plurality of microcells 202 are embedded inside the low refractive index portion 201. Also, according to this configuration, it is possible to manufacture the optical arithmetic device without exposing the plurality of microcells 202 to air.

[0110] [Second Reference Form] A gel 20G according to a second embodiment of the present invention will be described with reference to Fig. 12. Fig. 12 is a schematic diagram of the gel 20G. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the explanations thereof will not be repeated.

[0111] The gel 20G is an example of a gel for manufacturing a microstructure for manufacturing the above-mentioned structure 20 or the optical diffraction element 20A. The gel 20G contains water and a triblock copolymer in which the first segments 211 and the second segments 212, each of which is composed of one or more block polymers, are alternately bonded to each other, and the total number of segments is three. Note that the triblock copolymer may be a multi-block copolymer as described above.

[0112] The gel 20G is obtained by dispersing a triblock copolymer 21, which includes a segment 211 and a segment 212 and in which a dye 22 is not bound to the segment 212, in water, which is an example of a hydrophilic solvent, and thereby swelling the triblock copolymer 21.

[0113] The triblock copolymer 21 is configured to be composed of segments 211 having hydrophobic properties at both ends, and a hydrophilic segment 212 is interposed between the segments 211. By dispersing such a triblock copolymer 21 in water, a polymer matrix 24 as shown in FIG. 12 is formed. The polymer matrix 24 is composed of water as a solvent, pseudo cross-linking points 241 formed by aggregation of the segments 211, and segments 212 interposed between the two cross-linking points 241. Note that in FIG. 12, the polymer matrix 24 is illustrated as a two-dimensional structure to make the structure of the polymer matrix easier to understand, but the actual polymer matrix 24 has a three-dimensional structure.

[0114] As described above, the segment 211 and the segment 212 constituting the triblock copolymer 21 can be produced by using a precision polymerization method. Therefore, the block polymers constituting the segment 211 and the segment 212 have a small molecular weight dispersion. The molecular weight dispersion of the block polymers of the segment 211 and the segment 212 is, for example, preferably 2 or less, and more preferably 1.2 or less. In this way, by precisely controlling the degree of polymerization of each of the segment 211 and the segment 212, it is possible to suppress the variation that may occur in the pitch p between the crosslinking points 241 in the polymer matrix 24.

[0115] In this embodiment, the polymer matrix 24 is formed using a triblock copolymer in which the segments 211 are located at both ends and the segments 212 are interposed between the segments 211, so water, which is an example of a hydrophilic solvent, is used as the solvent. Examples of hydrophilic solvents other than water include dimethyl sulfoxide (DMSO) and dimethylformamide (DMF).

[0116] Furthermore, when the polymer matrix 24 is formed using a triblock copolymer in which the segments 212 are located at both ends and the segments 211 are interposed between the segments 212, a hydrophobic solvent may be used as the solvent. Examples of the hydrophobic solvent include normal hexane and cyclohexane.

[0117] [Fourth embodiment] A manufacturing method M20 according to a fifth embodiment of the present invention, which is suitable for manufacturing the optical diffraction element 20A shown in FIG. 10, will be described with reference to FIG. 13 and FIG. 14. FIG. 13 is a flowchart of the manufacturing method M20. FIG. 14 is a schematic diagram of the gel 20G or the optical diffraction element 20A in each step included in the manufacturing method M20. FIG. 14(a) is a schematic diagram of the gel 20G after the dye dispersion step S12, FIG. 14(b) is a schematic diagram of the gel 20G in the exposure step S13, FIG. 14(c) is a schematic diagram of the gel 20G after the nanoparticle addition step S15, FIG. 14(d) is a schematic diagram of the gel 20G after the nanoparticle growth step S17, and FIG. 14(e) is a schematic diagram of the optical diffraction element 20A obtained by carrying out the dehydration and sintering step S18. For the sake of convenience, the same reference numerals are used to designate members having the same functions as those described in the above embodiment, and the description thereof will not be repeated. m It is based on the pFab method and uses a gel 20G containing a triblock copolymer 21.

[0118] As shown in FIG. 13, the manufacturing method M20 includes a gelling step S11, a dye dispersion step S12, an exposure step S13, a dye washing step S14, a nanoparticle adding step S15, a nanoparticle washing step S16, a nanoparticle growing step S17, and a dehydration / sintering step S18.

[0119] The gelation step S11 is a step of obtaining a gel 20G in which a triblock copolymer 21, in which first segments 211 and second segments 212 are alternately bonded and the total number of segments is 3, is swollen in water. Note that in the gelation step S11 of the present embodiment, the gel 20G is prepared using the triblock copolymer 21, but a multiblock copolymer in which the total number of segments is 4 or more may be used instead of the triblock copolymer 21.

[0120] The triblock copolymer 21 (see, for example, (a) of FIG. 9) including the segment 211 and the segment 212 can be appropriately purchased from among commercially available products, taking into consideration the degrees of polymerization of the segment 211 and the segment 212. In addition, the segment 211 and the segment 212 having the desired degrees of polymerization may be produced by a precision polymerization method, and then the triblock copolymer 21 may be produced using these.

[0121] First, an N,N-dimethylformamide (DMF) solution of the triblock copolymer 21 is prepared. The concentration of the triblock copolymer 21 is not particularly limited, but is, for example, 20% by weight. The solution is filled into a mold having a predetermined shape (rectangular in this embodiment). Next, a weak gel of the triblock copolymer 21 is obtained by exposing the surface of the solution to water vapor for several minutes. Next, the weak gel is immersed in water for three days to obtain a gel 20G.

[0122] If the gel 20G containing the desired triblock copolymer 21 is commercially available, it may be purchased and the gelling step S11 may be omitted.

[0123] The dye dispersion step S12 is one aspect of the first step, and is a step of dispersing a dye 22 in a gel 20G (see FIG. 14(a)). In FIG. 14, the segment 211 constituting the triblock copolymer 21 is shown by double lines, and the segment 212 is shown by solid lines. Also, the reference numerals 111 and 112 are omitted from the illustration. The dye 22 used in this embodiment is fluorescein shown in FIG. 9(b) in which the carboxyl group is replaced with an aminomethyl group.

[0124] The exposure step S13 is an embodiment of the second step, and is a step of patterning a predetermined region of the triblock copolymer 21 constituting the gel 20G in which the dye 22 is dispersed by exposing it to light (see FIG. 14(b)). The two-dot chain line shown in FIG. 14(b) shows a schematic representation of the region to be exposed. By absorbing the energy of the light irradiated by this exposure, the dye 22 bonds to the block polymer constituting the segment 212 (see FIG. 9(b)). In the gel 20G, which is a rectangular parallelepiped, a two-photon absorption exposure process is suitable for exposing a desired region three-dimensionally. By controlling the amount of exposure in the exposure step S13, the amount of dye 22 bonded to the segment 212 can be controlled. Thus, for example, in the subcell 202 of the microcell 202 shown in FIG. 11 ,202 12 ,202 21 ,202 22 In the region corresponding to the subcell having a high refractive index, the amount of exposure may be set high, and in the region corresponding to the subcell having a low refractive index, the amount of exposure may be set low.

[0125] The exposure step S13, the nanoparticle addition step S15, the nanoparticle washing step S16, the nanoparticle growth step S17, and the dehydration and sintering step S18, which will be described later, are performed in the same manner as in the I m These steps are known as the pFab method, and therefore, in this embodiment, only a brief explanation of these steps will be given.

[0126] The dye washing step S14 is one aspect of the third step, and is a step of washing the gel 20G after patterning to remove the unreacted dye 22 remaining in the gel 20G. By carrying out this step, only the dye 22 bound to the segment 212 in the exposed area remains inside the structure 20. In other words, the dye 22 remains only in the area patterned by exposure.

[0127] The nanoparticle addition step S15 is a step of modifying the dye 22 with nanoparticles 25 (eg, made of gold) (see FIG. 14(c)).

[0128] The nanoparticle washing step S16 is a step of washing the gel 20G after the dye 22 has been modified with the nanoparticles 25 to remove the nanoparticles that are not bound to the dye 22 and remain in the gel 20G.

[0129] The nanoparticle growth step S17 is a step of increasing the content of the high refractive index material in the gel 20G by further growing the nanoparticles 25 modified with the dye 22 (see FIG. 14(d)). In FIG. 14(d), the nanoparticles 25 are shown by dashed lines, and the particles 26 after growth are shown by solid lines.

[0130] The dehydration and sintering step S18 is an embodiment of the fourth step, and is a step of removing water from the triblock copolymer 21 from which the dye 22 has been removed, thereby shrinking the triblock copolymer 21 and obtaining the optical diffraction element 20A (see FIG. 14(e)). By carrying out this step, the gel 20G is reduced in size while maintaining a shape similar to that of the gel 20G before dehydration. In FIG. 14(e), the reduction ratio is set for convenience so that the size of the gel 20G is reduced to 1 / 2 by dehydration. However, the reduction ratio of the actual gel 20G due to dehydration is determined depending on the structure of the triblock copolymer 21 and the water content in the gel 20G (in other words, the degree of swelling). For example, in the triblock copolymer 21 of this embodiment (see FIG. 9(a)), when the water content in the gel 20G is about 83%, the reduction ratio due to dehydration is about 1 / 10.

[0131] At this time, as shown in FIG. 12, since there is little variation in the pitch p between the crosslinking points 241 in the polymer matrix 24 constituting the gel 20G, it is possible to suppress distortion that may occur with the contraction of the gel 20G. As a result, the area patterned in the exposure step S13 (the area shown by the two-dot chain line in FIG. 14(e)) is also reduced in size while maintaining a shape similar to that of the patterned area before dehydration. Therefore, in the optical diffraction element 20A manufactured using the manufacturing method M20, the conventional I mCompared to structures fabricated using the pFab method, distortion can be suppressed.

[0132] The dehydration and sintering step S18 is performed by heating the gel 20G after the nanoparticle growth step S17 in an oven. The temperature of the dehydration step is preferably set lower than the heat resistance temperature of the polymer used or the boiling point of the solvent in order to maintain a good shape. For example, in the case of a hydrogel based on water and acrylic acid, it is preferable to dry it at a temperature of 60°C to 95°C for about 30 to 120 minutes. It is also efficient to dry it in a vacuum after drying and shrinkage have progressed to a certain extent. The sintering temperature is preferably a temperature slightly lower than the melting point of the nanoparticles, and it is preferable to heat it as quickly as possible so as to melt only the surface of the nanoparticles. Exposure to high heat for a long period of time is likely to cause problems such as damage to the gel and oxidation of the metal nanoparticles. To prevent oxidation of the metal nanoparticles, sintering in an inert atmosphere or in a vacuum is preferable. Furthermore, the dehydration and sintering process may be a combination of a plurality of heating conditions. For example, in the first half of the dehydration process, the heating temperature of the oven is set to 90° C. and the heating time is set to 1 hour under atmospheric pressure to remove most of the water from the triblock copolymer 21, and then the mixture is dried for another 30 minutes while evacuating with a vacuum pump at the same temperature setting. In the subsequent sintering process, the heating temperature of the oven is changed to 400° C. and the heating time is changed to 3 minutes while continuing the evacuation, so that the particles 26 contained in the triblock copolymer 21 are sintered together. As a result, the particles 26 contained in the triblock copolymer 21 are fixed together, and the strength of the microcells 202 (see FIG. 10) in the optical diffraction element 20A can be increased. In addition, the sintering process is not limited to melting the nanoparticles by a heating method, and an instantaneous sintering method using irradiation with a laser or a flash xenon lamp may be adopted.

[0133] (summary) The optical diffraction element according to the first aspect of the present invention comprises a plurality of microcells arranged along a specific plane, each of which includes a plurality of subcells, and each subcell has a refractive index in at least one of the in-plane directions of the specific plane that is any one of n predetermined types of refractive indexes (n is an integer of 2 or more).

[0134] Since each microcell is composed of multiple subcells, the refractive index of each microcell is determined by the average value of the refractive indexes of the subcells. In addition, the refractive index of each subcell can be appropriately determined by selecting the refractive index of each microcell from among n predetermined types of refractive index. Since each microcell delays the phase of light passing through it according to its refractive index, a predetermined calculation can be optically performed by causing each light whose phase has been delayed according to the refractive index of each microcell to interfere with each other. Therefore, the present optical diffraction element can provide an optical diffraction element in which the refractive indexes of multiple microcells are individually set.

[0135] In addition, in the optical diffraction element according to the second aspect of the present invention, in addition to the configuration of the optical diffraction element according to the first aspect described above, a configuration is adopted in which each of the subcells has a substantially uniform thickness.

[0136] In the present optical diffraction element, the thickness of each subcell is substantially uniform, and therefore the thickness of each microcell is also substantially uniform. Therefore, compared with an optical diffraction element in which the thicknesses of the multiple microcells are individually set, the aspect ratio of each microcell can be made substantially uniform. Therefore, the present optical diffraction element can suppress deformation of the microcells caused by variations in the aspect ratio of each microcell, which may occur when optically shaping an optical diffraction element in which the thicknesses of the multiple microcells are individually set.

[0137] The thickness of each subcell being approximately uniform means, for example, that the thicknesses of all the subcells are within a range of ±10% of the average thickness.

[0138] In addition, in an optical diffraction element according to a third aspect of the present invention, in addition to the configuration of the optical diffraction element according to the first or second aspect described above, each of the sub-cells includes a multi-block copolymer in which a first segment composed of a block polymer containing a mesogenic group having liquid crystal properties and a second segment composed of a block polymer not containing the mesogenic group are alternately connected, the multi-block copolymer having at least a total number of segments of 2 or more, and a guide for self-organizing the multi-block copolymer, and the orientation direction of the mesogenic group in each of the sub-cells is any one of n predetermined orientation directions.

[0139] According to the above configuration, in each subcell, the mesogen group contained in the block polymer constituting the first segment has one of n predetermined orientation directions. The refractive index of the mesogen group changes depending on the angle between the long axis direction of the mesogen group and the polarization direction of linearly polarized light incident on the subcell. Therefore, when linearly polarized light is incident on the optical diffraction element, the refractive index of each subcell has one of n predetermined refractive indexes. In this way, in the optical diffraction element, the subcell can be realized by using a multiblock polymer containing a mesogen group in one segment and a guide.

[0140] Furthermore, in an optical diffraction element according to a fourth aspect of the present invention, in addition to the configuration of the optical diffraction element according to the third aspect described above, a configuration is adopted in which the surface of the guide has either a hydrophobic or hydrophilic polarity, and in the multi-block copolymer, one of the first segment and the second segment is hydrophobic and the other segment is hydrophilic.

[0141] According to the above configuration, the multi-block copolymer is arranged such that the first and second segments, which have the same polarity as the surface of the guide, are adjacent to the guide side, and the segments, which have a different polarity from the surface of the guide, are distant from the guide side. This allows the alignment direction of the mesogen groups to be reliably aligned, thereby allowing the refractive index in each subcell to be reliably controlled.

[0142] Furthermore, in an optical diffraction element according to a fifth aspect of the present invention, in addition to the configuration of the optical diffraction element according to the first or second aspect described above, a configuration is adopted in which each subcell contains a polymer matrix made of a polymer, and a part of the polymer has bound dye, dye, and nanoparticles bound to it in that order, and the refractive index of the nanoparticles is greater than the refractive index of the polymer matrix.

[0143] According to the above configuration, the amount or concentration of the dye and nanoparticles to be bonded to the polymer is determined in n types, and the amount or concentration of the dye and nanoparticles is selected from the n types for each subcell, so that the refractive index of the subcell can be set to one of the n predetermined refractive indices. In this manner, in the present optical diffraction element, the subcell can be realized by using a polymer matrix composed of a polymer to which the dye and nanoparticles are bonded.

[0144] In addition, in an optical diffraction element according to a sixth aspect of the present invention, in addition to the configuration of the optical diffraction element according to the fifth aspect described above, the polymer matrix is ​​composed of first and second segments, each of which is composed of one or more block polymers, and the first and second segments, each of which has hydrophobicity and hydrophilicity, are alternately bonded to each other, and is composed of a multi-block copolymer having a total number of segments of 3 or more, and in each multi-block copolymer, a dye and nanoparticles are bonded to the first segment or the second segment in this order, and the refractive index of the nanoparticles is greater than the refractive index of the polymer matrix.

[0145] According to the above configuration, a multi-block copolymer is used as a polymer constituting the polymer matrix. The block polymers constituting each of the first and second segments have a linear form, but since hydrophobic and hydrophilic segments are alternately bonded and the total number of segments is 3 or more, when dispersed in a hydrophilic or hydrophobic solvent, the segments having the opposite polarity to the solvent aggregate in the solvent, and this site becomes a physical crosslinking point, and a swollen gel form can be obtained. For example, when a block polymer consisting of three segments, a hydrophobic segment / hydrophilic segment / hydrophobic segment, is dispersed in water, the hydrophobic segments at both ends of the multiple block polymers aggregate together and become physical crosslinking points, thereby forming a gel form. Meanwhile, since the block polymers constituting each of the first and second segments can be manufactured using a precision polymerization method, the molecular weight distribution of each of the first and second segments can be reduced. Therefore, in a gel obtained by swelling the multi-block copolymer with a solvent, the variation that may occur in the pitch between the crosslinking points in the polymer matrix can be suppressed. Therefore, the present optical diffraction element has a structure different from that of the conventional I. m In comparison with an optical diffraction element manufactured using the pFab method, distortion that may occur in the subcell can be suppressed.

[0146] In addition, in an optical diffraction element according to a seventh aspect of the present invention, in addition to the configuration of the optical diffraction element according to the sixth aspect described above, the multi-block copolymer is a triblock copolymer having a total number of segments of 3, and is composed of two of the first segments and a second segment interposed between the two first segments.

[0147] According to the above arrangement, a hydrophilic solvent (for example, water) can be used as the solvent for swelling the multi-block copolymer.

[0148] Furthermore, in an optical diffraction element according to an eighth aspect of the present invention, in addition to the configuration of the optical diffraction element according to any one of the first to seventh aspects described above, a configuration is adopted in which each microcell changes the phase of light when light having a predetermined wavelength λ is incident on it in accordance with the refractive index of the microcell, and the cell size of each microcell is equal to or smaller than the wavelength λ.

[0149] According to the above configuration, each microcell can delay the phase of light having a wavelength λ.

[0150] Furthermore, in an optical diffraction element according to a ninth aspect of the present invention, in addition to the configuration of the optical diffraction element according to the eighth aspect described above, a configuration is adopted in which the cell size of each of the microcells is equal to or smaller than the wavelength λ.

[0151] According to the above configuration, each microcell can efficiently delay the phase of light having the wavelength λ.

[0152] An optical computing device according to a tenth aspect of the present invention has N (N is an integer of 2 or more) optical diffraction elements according to any one of the first to ninth aspects described above, and the areas in which the multiple microcells of each optical diffraction element are provided overlap with each other.

[0153] According to the above configuration, an optical arithmetic unit can be realized by using an optical diffraction element in which the refractive indexes of a plurality of microcells are individually set.

[0154] A method for producing an optical diffraction element according to an eleventh aspect of the present invention is a method for producing an optical diffraction element including a plurality of microcells, each of which includes a plurality of subcells. In this method, each subcell includes a multi-block copolymer in which a first segment formed of a block polymer containing a mesogen group having liquid crystallinity and a second segment formed of a block polymer not containing the mesogen group are alternately connected, the multi-block copolymer having at least two total segments, and a guide for self-organizing the multi-block copolymer, and the method includes the steps of providing the guide on a main surface of a substrate and forming the multi-block copolymer so as to cover the guide, so that the orientation direction of the mesogen group in each subcell is one of n predetermined orientation directions.

[0155] According to the above configuration, the same effects as those of the optical diffraction element according to the third aspect described above can be achieved.

[0156] [Additional Notes] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. [Explanation of symbols]

[0157] 1 Optical calculation device 10, 10a, 10b, 10c Optical diffraction element 11 Microcell Group 11 ij Microcell 12 Subcell Group 12 kl Subcell 12g,12g kl guide 12P,12P kl Diblock Copolymer S1,S2 segment 20 Structure 20A Optical Diffraction Element 20G gel (an example of gel for manufacturing microstructures) 201 Low refractive index section 202 Microcell 202 11 ,202 12 ,202 21 ,202 22 Subcell 21 Triblock copolymer (an example of a multi-block copolymer) 211, 212 segments (examples of the first and second segments) 22 Dye 23 Crosslinking material 24 Polymer Matrix 241 Crosslinking point

Claims

1. a plurality of microcells arranged along a particular plane, each microcell including a plurality of subcells; Each subcell has a refractive index in at least one direction among in-plane directions of the specific plane, the refractive index being one of n predetermined types of refractive indexes (n is an integer of 2 or more) that are numerically classified; Each of the subcells includes a guide; The guide is A first member extending in a first direction on the specific plane; a second member extending in a second direction on the particular plane, the second member being different from the first direction; 1. An optical diffraction element comprising:

2. The first member and the second member have different lengths.

2. The optical diffraction element according to claim 1 .

3. The optical diffraction element is A plurality of the first members; a plurality of the second members intersecting the plurality of the first members; The boundaries of each subcell are A pair of first members adjacent to each other; A pair of second members adjacent to each other; It is stipulated by In each subcell, one of the pair of first members and the pair of second members each having a notch; 2. The optical diffraction element according to claim 1 .

4. In at least some of the subcells, one of the pair of members, which is the other of the pair of first members and the pair of second members, has a notch; 4. The optical diffraction element according to claim 3.

5. In at least some of the subcells, the other member of the pair of members is continuous; 5. The optical diffraction element according to claim 4.

6. each of the subcells has a thickness within a range of ±10% of the average thickness of all the subcells; 2. The optical diffraction element according to claim 1 .

7. Each of the subcells comprises: a multi-block copolymer in which first segments constituted by block polymers containing mesogen groups having liquid crystal properties and second segments constituted by block polymers not containing mesogen groups are alternately connected, and the total number of segments is at least 2; The guide causes the multi-block copolymer to self-assemble; an alignment direction of the mesogen group in each of the subcells is any one of n predetermined alignment directions corresponding to the n predetermined refractive indexes, 3. The optical diffraction element according to claim 1, wherein the first and second optical components are arranged in a first plane.

8. The surface of the guide has either hydrophobic or hydrophilic polarity; In the multi-block copolymer, one of the first segment and the second segment is hydrophobic and the other segment is hydrophilic.

8. The optical diffraction element according to claim 7.

9. Each subcell contains a polymer matrix comprised of a polymer; a part of the polymer has a bound dye and a nanoparticle bound thereto, in that order; the refractive index of the nanoparticles is greater than the refractive index of the polymer matrix; 3. The optical diffraction element according to claim 1, wherein the first and second optical components are arranged in a first plane.

10. the polymer matrix is ​​composed of a multi-block copolymer in which first and second segments, each of which is composed of one or more block polymers, are alternately bonded to the first and second segments, each of which has hydrophobicity and hydrophilicity, and the total number of segments is 3 or more; In each multiblock copolymer, a dye and a nanoparticle are bound to the first segment or the second segment in this order; the refractive index of the nanoparticles is greater than the refractive index of the polymer matrix; 10. The optical diffraction element according to claim 9.

11. The multi-block copolymer is a triblock copolymer having a total number of segments of 3, and is composed of two of the first segments and a second segment interposed between the two first segments.

11. The optical diffraction element according to claim 10.

12. Each microcell changes the phase of light having a predetermined wavelength λ in response to the refractive index of the microcell.

12. The optical diffraction element according to claim 1, wherein the first and second optical elements are arranged in a first plane.

13. The cell size of each microcell is equal to or smaller than the wavelength λ.

13. The optical diffraction element according to claim 12.

14. A system including N (N is an integer of 2 or more) optical diffraction elements according to any one of claims 1 to 13, The regions in which the plurality of microcells of each optical diffraction element are provided overlap each other. An optical computing device comprising:

15. 1. A method of manufacturing an optical diffractive element comprising a plurality of microcells, each microcell comprising a plurality of subcells, the method comprising the steps of: Each subcell includes a multi-block copolymer in which a first segment formed of a block polymer containing a mesogen group having liquid crystal properties and a second segment formed of a block polymer not containing a mesogen group are alternately connected, the multi-block copolymer having a total number of segments of at least 2, and a guide for self-organizing the multi-block copolymer; The guide is A first member extending in a first direction on a particular plane; a second member extending in a second direction on the particular plane, the second direction being different from the first direction; providing the guide on a main surface of the substrate so that the alignment direction of the mesogen groups in each of the subcells is one of n predetermined alignment directions; and forming the multi-block copolymer over the guide.

4. A method for producing an optical diffraction element comprising the steps of:

Citation Information

Patent Citations

  • Water-based crosslinkable resin composition

    JP2002275224A

  • Polymer for birefringence-inducing material, polarization diffraction element, and liquid crystal alignment film

    JP2005232345A

  • Porous holographic film

    JP2008523453A

  • Polarization gratings in mesogenic films

    JP2008532085A

  • Structured-groove diffraction granting and method for control and optimization of spectral efficiency

    US20060050391A1