METHOD FOR PRODUCING AROMATIC POLYCYCLIC FUNCTIONAL COMPOUND, NOVEL AROMATIC POLYCYCLIC FUNCTIONAL COMPOUND, ORGANIC SEMICONDUCTOR INK, AND ORGANIC SEMICONDUCTOR DEVICE

A novel synthetic method for aromatic polycyclic fused ring compounds addresses the challenge of limited electron-donating sites and noble metal residues, enabling high EQE in organic semiconductor devices by producing n-type compounds with enhanced electron donating properties.

JP7555538B2Active Publication Date: 2024-09-25MITSUBISHI CHEM CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020130217
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-31
Publication Date
2024-09-25
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

The synthesis of aromatic polycyclic fused ring compounds with high electron donating properties for improving photoelectric conversion efficiency in near-infrared regions is challenging due to limited electron-donating sites and the use of noble metals, which can leave residues in the compound.

Method used

A novel synthetic method involving a reaction between a compound, divalent iron, trivalent phosphorus, and magnesium, without using precious metals, to produce aromatic polycyclic condensed rings with high electron donating properties, which are incorporated into n-type compounds for organic semiconductor devices.

Benefits of technology

This method enables the production of organic semiconductor devices with high external quantum efficiency (EQE) by using n-type compounds with improved electron donating moieties, enhancing photoelectric conversion in the near-infrared region.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555538000001
    Figure 0007555538000001
  • Figure 0007555538000002
    Figure 0007555538000002
  • Figure 0007555538000003
    Figure 0007555538000003
Patent Text Reader

Abstract

To provide a new production method for an aromatic polycyclic condensed compound having high electron-donating properties.SOLUTION: A method for producing an aromatic polycyclic condensed compound, illustrated in Embodiment 1, includes a reaction step in which a compound 5 of an acetylene structure, a bivalent iron compound, a trivalent phosphorus compound, and magnesium are made to coexist and subjected to an oxidation reaction.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aromatic polycyclic fused ring compound, a novel aromatic polycyclic fused ring compound, an organic semiconductor ink, and an organic semiconductor device. [Background technology]

[0002] The roles required of image sensors are becoming more diverse, with increasing opportunities for use in machine processing for motion recognition, spatial measurement, spatial mapping, shape recognition, etc. For recognition by sensors, not only visible light but also reflected infrared light that cannot be sensed by humans is processed, but the photoelectric conversion efficiency in the near-infrared region has been insufficient (see, for example, Non-Patent Documents 1 and 2).

[0003] To improve the photoelectric conversion efficiency (external quantum efficiency) in the near-infrared region, studies have been conducted so far on the principle of CMOS photoelectric conversion, in which the photoelectric conversion layer absorbs light to generate excitons and separate charges, thereby creating a photoelectric conversion layer with high absorbance and improved internal quantum efficiency, or on making the photoelectric conversion layer thicker to improve absorbance.

[0004] Non-Patent Document 3 describes a non-fullerene compound with a narrowed band gap and a method for synthesizing the same. This non-fullerene compound has a skeleton with an electron-donating site in the center of the molecule and electron-withdrawing sites on both sides. In order to improve the photoelectric conversion efficiency (external quantum efficiency) in the near-infrared region, based on the principle of CMOS photoelectric conversion, the photoelectric conversion layer absorbs light to generate excitons and separate charges, so that it is necessary to make the photoelectric conversion layer have high absorbance with improved internal quantum efficiency, or to increase the thickness of the photoelectric conversion layer to improve absorbance, but it is difficult to synthesize a site that serves as a sufficient electron-donating group, and the types of preferred electron-donating sites have been limited (see Non-Patent Document 3). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] DOI:10.1021 / acs.chemmater.9b00966,Chem.Mater.(2019) [Non-Patent Document 2] ACS Appl.Mater.Interfaces 2018,10,11063-11069. [Non-Patent Document 3] Adv.Energy Mater.,2018,8,1801212. Summary of the Invention [Problem to be solved by the invention]

[0006] Molecular design of n-type semiconductors for use in semiconductor devices with higher photoelectric conversion efficiency has been underway, but the synthesis of the electron-donating moiety skeleton has been difficult. Furthermore, these electron-donating moieties use coupling reactions using precious metals, which has the problem of precious metals remaining in the compound. In order to improve the external quantum efficiency of organic semiconductor devices such as near-infrared sensors, it is necessary to extend the wavelength of the absorption region, and it has been essential to establish a method for synthesizing aromatic polycyclic fused ring compounds with high electron-donating properties. The objective of the present invention is to provide a new method for producing aromatic polycyclic fused ring compounds with high electron-donating properties. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have developed an electron donor that does not use a noble metal. The inventors established a synthetic method for aromatic polycyclic fused rings, which are electron-donating moieties, with a wide range of applications, and used the synthetic method to produce novel compounds. Furthermore, they discovered that an organic semiconductor device with high external quantum efficiency (EQE) can be obtained by producing an n-type compound incorporating the electron-donating moiety and constructing an organic semiconductor device having an active layer containing a p-type conjugated polymer and the n-type compound, thereby completing the present invention. That is, the gist of the present invention is as follows.

[0008] (1) A method for producing an aromatic polycyclic fused ring compound represented by the following formula (II), comprising a reaction step of causing an oxidation reaction in the coexistence of a compound represented by the following formula (I), a divalent iron compound, a trivalent phosphorus compound, and magnesium. [ka] (In formula (I) and formula (II), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; Ar 1 , and Ar 2 are each independently selected from aromatic hydrocarbons and aromatic heterocycles having a 5- or 6-membered ring, which may have a substituent. 1 , Z 2 , Z 3 , and Z 4 are each independently selected from a silyl group or a methyl group which may have a substituent, and n represents an integer of 0 or more. (2) The method according to (1), wherein in the reaction step, lithium halide is allowed to coexist when the magnesium cyclized product is formed. (3) The method according to (1) or (2), wherein in the reaction step, the oxidation reaction uses at least one selected from the group consisting of air, oxygen, a halogen compound, and an organic peroxide as an oxidizing agent. (4) In the formula (II), Ar 1 and Ar 2 is a thiophene ring. (5) An aromatic polycyclic fused ring compound represented by the following formula (II)': [ka] (In formula (II)', R 1 , R 2 , R 3 , R 4, R 5 , R 6 , R 7 , and R 8 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; Ar 1 and Ar 2 is a thiophene ring, and n is an integer of 0 or more. (6) A method for producing an n-type semiconductor compound represented by the following general formula (III), which is produced by reacting the compound according to (5) as an intermediate: [ka] (In formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 is the same as in formula (II)', R 9 , R 10 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; 1 , X 2 each independently represents a halogen atom, p and q each independently represent an integer from 0 to 4, r and s each independently represent 0 or 1, and n represents an integer of 0 or more. (7) An organic semiconductor device comprising an active layer containing a p-type conjugated polymer and an n-type compound represented by the following general formula (III): [ka] (In formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group;1 , X 2 each independently represents a halogen atom, p and q each independently represent an integer from 0 to 4, r and s each independently represent 0 or 1, and n represents an integer of 0 or more. (8) The organic semiconductor device according to (7), wherein the active layer contains at least one fullerene compound selected from the group consisting of

[60] fullerene,

[70] fullerene,

[60] PCBM,

[70] PCBM, bis

[60] PCBM, bis

[70] PCBM,

[60] SIMEF,

[70] SIMEF,

[60] ICBA,

[70] ICBA,

[60] ICMA, and

[70] ICMA. (9) The organic semiconductor device according to (7) or (8), wherein the active layer contains a polycyclic aromatic compound or 1,8-diiodooctane. (10) The organic semiconductor device according to any one of (7) to (9), which is a photoelectric conversion element. (11) The organic semiconductor device according to any one of (7) to (10), which has an external quantum efficiency (EQE) of 50% or more when irradiated with light having a wavelength of 940 nm. (12) An organic semiconductor ink comprising: a p-type conjugated polymer; an n-type compound represented by formula (III); at least one fullerene compound selected from the group consisting of

[60] fullerene,

[70] fullerene,

[60] PCBM,

[70] PCBM, bis

[60] PCBM, bis

[70] PCBM,

[60] SIMEF,

[70] SIMEF,

[60] ICBA,

[70] ICBA,

[60] ICMA, and

[70] ICMA; and a solvent, wherein the weight ratio of the fullerene compound to the n-type compound is 2.0 or less. (13) The organic semiconductor ink according to (12), which contains a polycyclic aromatic compound and / or 1,8-diiodooctane. (14) A photodetector using the organic semiconductor device according to any one of (7) to (11). (15) The photodetector according to (14), which is used to detect light having a wavelength of 700 to 1200 nm. Effect of the Invention

[0009] According to the present invention, a new method for producing an aromatic polycyclic fused ring compound having high electron-donating properties is provided. The aromatic polycyclic fused ring compound produced by the method includes a novel aromatic polycyclic fused ring compound. Furthermore, the compound obtained by the method has an aromatic polycyclic fused ring containing a highly electron-donating moiety and can be used as an n-type low molecular weight compound for organic semiconductor devices. Furthermore, by using this, it is possible to provide organic semiconductor devices with high external quantum efficiency (EQE). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described, but the embodiment of the present invention is not limited to the following embodiment.

[0011] One aspect of the present invention is a method for producing an aromatic polycyclic fused ring compound represented by formula (II) below, comprising a reaction step of causing a compound represented by formula (I) below, a divalent iron compound, a trivalent phosphorus compound, and magnesium to coexist, forming a magnesium cyclized product in a system, and carrying out an oxidation reaction. [ka]

[0012] In formula (I) and formula (II), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from an alkyl group which may have a substituent, and an aromatic ring group which may have a substituent. Examples of the alkyl group include linear, branched or cyclic alkyl groups such as methyl, ethyl, n-propyl, n-butyl, 2-methylpropyl, 2-methylbutyl, 3-methylbutyl, cyclohexylmethyl, neopentyl, 2-ethylbutyl, isopropyl, 2-butyl, cyclohexyl, 3-pentyl, tert-butyl, 1,1-dimethylpropyl, 2-ethylhexyl, 2-butyloctyl, etc. Among these, alkyl groups having 20 or less carbon atoms are preferred.

[0013] Examples of the aromatic group include aryl groups such as phenyl, naphthyl, anthranyl, fluorenyl, phenanthrenyl, and azulenyl, and heteroaryl groups such as thienyl, imidazolyl, pyrazolyl, and thiazolyl. Among these, preferred are monocyclic or two-condensed ring aryl groups or monocyclic heteroaryl groups having 12 or less carbon atoms. More preferred are monocyclic aryl groups or thienyl groups having 6 or less carbon atoms.

[0014] Examples of the substituent of the group which may have a substituent include a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heteroaryl group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an alkylthio group, an aryloxy ... Examples of such groups include an arylthio group, a heteroarylthio group, an amino group, an acyl group, an aminoacyl group, a ureido group, a sulfonamide group, a carbamoyl group, a sulfamoyl group, a sulfamoylamino group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, a heteroarylsulfonyl group, an imido group, and a silyl group.

[0015] Specifically, alkyl groups having about 1 to 15 carbon atoms, such as methyl and ethyl groups; Alkenyl groups having about 2 to 10 carbon atoms, such as ethynyl and propylenyl groups; Alkynyl groups with 2 to 10 carbon atoms, such as acetylenyl groups; Aryl groups having about 6 to 20 carbon atoms, such as phenyl and naphthyl groups; Heteroaryl groups having about 3 to 20 carbon atoms, such as thienyl, furyl, and pyridyl groups; Alkoxy groups having about 1 to 15 carbon atoms, such as a methoxy group, an ethoxy group, or a propoxy group; Aryloxy groups having about 6 to 20 carbon atoms, such as phenoxy and naphthoxy groups; Heteroaryloxy groups having about 3 to 20 carbon atoms, such as a pyridyloxy group and a thienyloxy group; Alkylthio groups having about 1 to 15 carbon atoms, such as methylthio and ethylthio groups; Arylthio groups having about 6 to 20 carbon atoms, such as a phenylthio group and a naphthylthio group; Heteroarylthio groups having about 3 to 20 carbon atoms, such as a pyridylthio group and a thienylthio group; an amino group having about 1 to 20 carbon atoms, such as a dimethylamino group or a diphenylamino group, which may have a substituent; Acyl groups having about 2 to 20 carbon atoms, such as acetyl and pivaloyl groups; Acylamino groups having about 2 to 20 carbon atoms, such as an acetylamino group or a propionylamino group; ureido groups having about 2 to 20 carbon atoms, such as a 3-methylureido group; Sulfonamide groups having about 1 to 20 carbon atoms, such as methanesulfonamide groups and benzenesulfonamide groups; Carbamoyl groups having about 1 to 20 carbon atoms, such as a dimethylcarbamoyl group and an ethylcarbamoyl group; Sulfamoyl groups having about 1 to 20 carbon atoms, such as ethylsulfamoyl groups; Sulfamoylamino groups having about 1 to 20 carbon atoms, such as a dimethylsulfamoylamino group; alkoxycarbonyl groups having about 2 to 6 carbon atoms, such as a methoxycarbonyl group and an ethoxycarbonyl group; Aromatic hydrocarbon oxycarbonyl groups having about 7 to 20 carbon atoms, such as phenoxycarbonyl and naphthoxycarbonyl groups; Aromatic heterocyclic hydrocarbon oxycarbonyl groups having about 6 to 20 carbon atoms, such as pyridyloxycarbonyl groups; Alkylsulfonyl groups having about 1 to 6 carbon atoms, such as a methanesulfonyl group, an ethanesulfonyl group, or a trifluoromethanesulfonyl group; Arylsulfonyl groups having about 6 to 20 carbon atoms, such as benzenesulfonyl groups and monofluorobenzenesulfonyl groups; Heteroaryloxysulfonyl groups having about 3 to 20 carbon atoms, such as thienylsulfonyl groups; imide groups having about 4 to 20 carbon atoms, such as phthalimide groups; Alternatively, a silyl group which is substituted with three substituents selected from the group consisting of an alkyl group and an aryl group can be mentioned.

[0016] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 Particularly preferred as the aryl group are an alkyl group having a total of 15 or less carbon atoms which may have a substituent, a monocyclic aryl group having a total of 20 or less carbon atoms which may have a substituent, and a monocyclic heteroaryl group having a total of 15 or less carbon atoms which may have a substituent.

[0017] Ar 1 , and Ar 2 are each independently selected from aromatic hydrocarbons and aromatic heterocycles having a 5- or 6-membered ring, which may have a substituent. 1 , Ar 2 are preferably each independently an optionally substituted aryl group or an optionally substituted heteroaryl group.

[0018] Specifically, the above R 1 ~R 8 Examples of the substituent of the optionally substituted group include the aryl group and the heteroaryl group mentioned above. 1 ~R 8 The same things as those given above can be given. Ar 1 , Ar 2More preferably, it is a monocyclic aryl group having a total of 15 or less carbon atoms which may have a substituent, or a monocyclic heteroaryl group having a total of 15 or less carbon atoms which may have a substituent. Particularly preferred is a thiophene ring which may have a substituent. Among the above-mentioned substituents, more preferred are an alkyl group having about 1 to 15 carbon atoms, an alkoxy group having about 1 to 15 carbon atoms, and a halogen atom.

[0019] In formula (1), Z 1 , Z 2 , Z 3 , and Z 4 are each independently selected from a silyl group or a methyl group which may have a substituent. Examples of the silyl group include a trimethylsilyl group, a triethylsilyl group, a t-butyldiphenylsilyl group, a n-butyldimethylsilyl group, a dimethylethylsilyl group, a dimethylphenylsilyl group, a dimethylisopropylsilyl group, a triisopropylsilyl group, and a tert-butyldimethyl group. Particularly preferred are a methoxy group or a trimethylsilyl group, which have little steric hindrance.

[0020] n represents an integer of 0 or more, and is preferably an integer of 0 to 5.

[0021] (Divalent iron compounds) The "divalent iron compound" that is allowed to coexist with the compound of formula (I) in the reaction step of this embodiment means that the iron in the compound is divalent. Examples of the divalent iron compound include compounds such as FeCl2, FeBr2, FeI2, Fe(OAc)2, and Fe(acac)2. The amount of the divalent iron compound to be coexisted in the reaction step is not particularly limited, but is within the range of 1 mol% to 30 mol%, and more preferably 1 mol% to 20 mol%, relative to the compound of general formula (I).

[0022] (Trivalent phosphorus compounds) The "trivalent phosphorus compound" that is allowed to coexist with the compound of formula (I) in the reaction step of this embodiment means that phosphorus in the compound is trivalent. The trivalent phosphorus compound is selected from the trivalent phosphorus ligands described in, for example, Sigma-Aldrich's "Buchwald Portfolio 2019 Palladacycles and Ligands" and "Pd Catalysts and Ligands Application Guide for Cross-Coupling Reactions". Among these, triphenylphosphine and tri(orthotolyl)phosphine are preferred because they can be used simply and inexpensively, and tri-tert-butylphosphine is preferred because it can increase reactivity. Buchwald phosphorus ligands are preferred because the yield of the compound of general formula (II) in the reaction of this form can be improved by selecting the optimal ligand depending on the substrate. It is preferable to use a trivalent phosphorus compound in a molar ratio of 1:1 to 1:3 relative to the divalent iron compound, and particularly preferably in a ratio of 1:1.5 to 1:2.5.

[0023] (magnesium) The magnesium that is allowed to coexist with the compound of formula (I) in the reaction step of this embodiment is not particularly limited, and may be magnesium metal or a magnesium-containing compound. Examples of magnesium-containing compounds include Rieke magnesium and turbo magnesium manufactured by Aldrich Co. The amount of magnesium to be coexisted is preferably 3 to 10 moles per mole of the compound of general formula (I), and more preferably 3 to 5 moles in order not to reduce the stirring efficiency in the system.

[0024] (Lithium Halide) In the reaction step of this embodiment, it is preferable to further coexist with lithium halide. By further coexisting with lithium halide, it is preferable to activate the magnesium reagent. Examples of lithium halide include lithium chloride, lithium bromide, and lithium iodide, and it is preferable to coexist these lithium halides in an equimolar amount with magnesium. Specifically, the molar ratio of magnesium:lithium halide is preferably 1:0.5 to 1:1.5, and more preferably 1:0.8 to 1:1.2.

[0025] (solvent) The reaction of this embodiment is usually carried out in a solvent. Examples of the solvent used at that time include Aromatic solvents such as toluene and chlorobenzene; Ethereal solvents such as ether, 1,4-dioxane, and THF; Aliphatic solvents such as hexane and heptane; The solvent can be selected from halogen-based solvents such as methylene chloride, chloroform, and 1,2-dichloroethane. Of these, toluene and tetrahydrofuran are preferably used. These solvents may be used alone or in combination of two or more. For example, when a solvent having low solubility of the substrate is used, the reaction results are improved by combining it with a halogen-based solvent or an ether-based solvent, and when a solvent having low dissolved oxygen concentration is used, the reaction results are improved by combining it with a non-polar solvent, more preferably a hydrocarbon-based solvent.

[0026] (Oxidizing agent) In the reaction step of this embodiment, it is preferable to carry out the oxidation reaction using an oxidizing agent. The oxidizing agent may be air, oxygen, or a halogen compound; for example, iodine, bromine, tetrabutylammonium tribromide, bromine-1,4-dioxane complex, 1,2-dibromo-1,1,2,2-tetrachloroethane, 1,2-dichloroethane pyridinium bromide perbromide, 1,8-diazabicyclo[5.4.0]-7-undecene hydrogen tribromide, NBS, 5,5-dibromo Meldrum's acid, trimethylsilyl bromide, 1-chloro-2-iodoethane, NIS, tetramethylammonium dichloroiodide, etc. peroxide, pyridine iodine monochloride, TMSI, organic peroxides; for example, diacyl peroxide, alkyl peroxy ester, peroxydicarbonate, peroxycarbonate, peroxyketal, dialkyl peroxide, alkyl hydroperoxide, mCPBA, t-butyl hydroperoxide, bis(trimethylsilyl) peroxide, di-t-butyl peroxide, 2-hydroperoxy-4,5-diphenyl-1,3,5-triazine, and methyl ethyl ketone peroxide. In order to suppress side reactions, an oxidizing agent having a weak nucleophilicity is preferred.

[0027] (Reaction temperature) The reaction temperature in the reaction step of this embodiment is usually -5°C or higher, preferably 0°C or higher, more preferably 10°C or higher, and particularly preferably in the range of about 25°C to the boiling point of the solvent, and can be arbitrarily set within the range up to the reflux temperature of the solvent used depending on the reaction rate. When the oxidation is slow (i.e., when the yield is poor), it is preferable to irradiate the reaction solution with ultrasound or microwaves, or to autoclave the reaction solution.

[0028] The reaction time is usually 30 minutes to 24 hours, but it depends on the type of solvent used and other reaction conditions, so it can be set arbitrarily. The progress of the reaction can be monitored by high-speed liquid crystal chromatograph. The reaction can be confirmed by using HPLC. After the reaction is completed, the target compound of general formula (II) can be obtained by using a known isolation and purification method. In order to remove the iron compound, it is preferable to further extract with a dilute aqueous hydrochloric acid solution.

[0029] The aromatic polycyclic fused ring compound represented by the general formula (II) can be produced by the above-mentioned method. Specific preferred examples of the compound represented by the above-mentioned general formula (II) are shown below.

[0030] [ka]

[0031] [ka]

[0032] [ka]

[0033] Another aspect of the present invention is a novel aromatic polycyclic fused ring compound represented by the following formula (II)'. [ka] In formula (II)', R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; Ar 1 , and Ar 2 is a thiophene ring, and n is an integer of 0 or more.

[0034] Another aspect of the present invention is a method for producing an n-type semiconductor compound, comprising the steps of preparing an aromatic polycyclic fused intercyclic compound represented by the above formula (II)', and producing a compound represented by the following general formula (III) using the above compound as an intermediate. [ka]

[0035] In formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 is the same as in formula (II), and R 9 , R 10 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; X 1 , X 2 each independently represents a halogen atom, and p and q each independently represent an integer from 0 to 4. r and s each independently represent 0 or 1, and n represents an integer of 0 or greater.

[0036] R 9 and R 10The alkyl group represented by the formula (I) is preferably a linear or branched alkyl group having 6 to 20 carbon atoms, more preferably 7 or more carbon atoms, even more preferably 8 or more carbon atoms, and still more preferably 15 or less carbon atoms, even more preferably 12 or less carbon atoms.

[0037] Examples of linear or branched hydrocarbon groups having 6 to 20 carbon atoms include linear alkyl groups such as n-octyl, n-decyl, lauryl, myristyl, and palmityl groups; branched primary alkyl groups such as 2-ethylhexyl and 2-butyloctyl groups; and branched secondary alkyl groups such as 2-octyl, 2-nonyl, and 2-decyl groups. Of these, R 9 and R 10 is preferably a primary branched chain hydrocarbon group.

[0038] X 1 and X 2 From the viewpoint of improving solubility, it is preferable that is a fluorine atom, and from the viewpoint of molecular arrangement when an active layer is formed, it is preferable that is a chlorine atom.

[0039] Each of r and s is preferably 1 or one of them is 0. Each of p and q is preferably 1 or 2. From the viewpoint of solubility, n is preferably 0 or 1.

[0040] The n-type compound represented by general formula (III) can be synthesized, for example, by the method described in Non-Patent Document 3 (Adv. Energy Mater., Vol. 8, 1801212 (2018)).

[0041] (n-type organic semiconductor compound) The compound of the above formula (III) can be incorporated as an n-type organic semiconductor compound into the active layer of an organic semiconductor device. The n-type compound represented by general formula (III) has an absorption maximum in solution in the range of 850 nm or more and 1200 nm or less, and has a band gap suitable for use as a photoelectric conversion element for an infrared photodetector. The active layer of the organic semiconductor device can contain an n-type fullerene compound and a p-type conjugated polymer in addition to the n-type organic semiconductor compound. Such an active layer of the organic semiconductor device is another embodiment of the present invention.

[0042] (n-type fullerenes) The active layer of the organic semiconductor device according to this embodiment may contain n-type fullerenes as an n-type organic semiconductor. The n-type fullerenes may be used alone or in combination of two or more. In this embodiment, by adding n-type fullerenes to the active layer containing a p-type conjugated polymer and an n-type compound, it is possible to improve the electron mobility and absorb the n-type compound in the near infrared region at the same time.

[0043] The n-type fullerenes are not particularly limited, and can be any known fullerenes as n-type semiconductors. Known fullerenes include fullerene-C60, fullerene-C70, fullerene-C76, fullerene-C78, fullerene-C84, fullerene-C240, fullerene-C540, mixed fullerene, fullerene nanotube, and other unmodified fullerenes; and fullerene derivatives in which a part of these is substituted with a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an aryl group, a heteroaryl group, a cycloalkyl group, a silyl group, an ether group, an amino group, a silyl group, or the like.

[0044] Specific fullerene derivatives include

[60] PCBM,

[70] PCBM, bis

[60] PCBM, bis

[70] PCBM,

[60] SIMEF,

[70] SIMEF,

[60] ICBA,

[70] ICBA,

[60] ICMA,

[70] ICMA, MP-C60,

[60] PCBiB,

[60] PCBH, and the like. Of these, the unmodified fullerene is preferably

[60] fullerene or

[70] fullerene.

[0045] Furthermore, the fullerene derivative is preferably

[60] PCBM,

[70] PCBM, bis

[60] PCBM, bis

[70] PCBM,

[60] SIMEF,

[70] SIMEF,

[60] ICBA,

[70] ICBA,

[60] ICMA, or

[70] ICMA, and more preferably

[60] PCBM,

[70] PCBM, or

[70] SIMEF.

[0046] The weight ratio of n-type fullerenes to the n-type compound in the active layer is not particularly limited, It is usually 0.2 or more, preferably 0.3 or more, more preferably 0.5 or more, and usually 2.0 or less, preferably 1.5 or less, more preferably 1.0 or less. By setting the weight ratio within the above range, the solubility of the active layer in the mixed solution can be ensured.

[0047] (p-type conjugated polymer) The active layer of the organic semiconductor device according to this embodiment contains a p-type conjugated polymer as a p-type organic semiconductor. For example, the p-type conjugated polymer may be a hole transporting polymer, and is preferably a hole transporting polymer having a structural unit that has a tendency to donate electrons. In addition, the p-type conjugated polymer is preferably one that can be mixed with an n-type organic semiconductor and coated to form a film.

[0048] In the hole transporting polymer, specific examples of a partial structure having excellent hole transporting properties include a benzodithiophene structure, a thiophene structure, a carbazole structure, a dibenzofuran structure, a triarylamine structure, a naphthalene structure, a phenanthrene structure, and a pyrene structure. A specific example of the p-type conjugated polymer is a p-type conjugated polymer represented by general formula (IV), in which n is a positive number.

[0049] [ka]

[0050] In the active layer, the weight ratio of the n-type compound to the p-type conjugated polymer is usually 0.5 or more, preferably 0.6 or more, more preferably 0.65 or more, and usually 1.5 or less, preferably 1.3 or less, more preferably 1.0 or less. In the active layer, the weight ratio of n-type fullerenes to p-type conjugated polymer is usually 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, and usually 2.0 or less, preferably 1.5 or less, more preferably 1.0 or less. The method for forming the active layer is not particularly limited, and the active layer can be formed by a known method, but is typically a coating method.

[0051] When forming an active layer by a coating method, an organic semiconductor ink is prepared by dissolving the organic semiconductor p-type conjugated polymer, n-type compound, and n-type fullerenes, as well as other necessary substances as additives, in an organic solvent, and the organic semiconductor ink is applied onto a substrate by a spin coating method or the like, and then dried to form the active layer. The spin coating conditions may be appropriately determined according to a standard method, taking into consideration the viscosity of the organic semiconductor ink, etc. The drying conditions are not particularly limited as long as the organic solvent in the organic semiconductor ink can be removed, and for example, the organic semiconductor ink can be dried by heating and annealing the organic semiconductor ink at 70°C to 130°C for 5 minutes to 20 minutes under atmospheric pressure. These organic semiconductor inks are also another embodiment of the present invention.

[0052] The contents of the p-type conjugated polymer, the n-type compound, and the n-type fullerenes in the organic semiconductor ink are not particularly limited as long as an active layer can be formed by coating. The content of the p-type conjugated polymer in the organic semiconductor ink is usually 0.5% by mass or more, and may be 0.7% by mass or more, and is usually 1.5% by mass or less, and may be 1.3% by mass or less. The content of n-type fullerenes in the organic semiconductor ink is usually 0.3% by mass or more, and may be 0.4% by mass or more, and is usually 1.5% by mass or less, and may be 1.0% by mass or less.

[0053] Furthermore, the content of the n-type compound in the organic semiconductor ink is typically 0.7% by mass or more, and may be 1.0% by mass or more, and is typically 2.0% by mass or less, and may be 1.8% by mass or less. In this embodiment, the weight ratio of n-type fullerenes to n-type compounds in the organic semiconductor ink is usually 0.3 or more, preferably 0.5 or more, more preferably 0.6 or more, and usually 2.0 or less, preferably 1.5 or less, more preferably 1.0 or less. By keeping the weight ratio within the above range, there is an effect of improving the EQE due to the high electron mobility of n-type fullerenes.

[0054] The organic solvent used in the organic semiconductor ink is not particularly limited, and organic solvents generally used in coating solutions for forming active layers of organic semiconductor devices can be used. Specifically, organic solvents such as halogen solvents such as chloroform and dichloroethane, aromatic hydrocarbon solvents such as toluene, xylene, chlorobenzene and dichlorobenzene, and ether solvents such as THF and dibutyl ether can be used. This is because organic semiconductors generally have high solubility in these organic solvents. In addition, the use of these organic solvents can be expected to improve photoelectric conversion efficiency.

[0055] Of the above organic solvents, the organic solvent is preferably xylene, chlorobenzene or chloroform, depending on the type of organic semiconductor. In addition, when adjusting the solubility, the organic solvent may be a mixed organic solvent of two or more kinds. The content ratio is not particularly limited, and may be in the range of 1:9 to 9:1. The difference in boiling point between these organic solvents is preferably 50°C or less, more preferably 40°C or less, and even more preferably 30°C or less.

[0056] In addition to the p-type conjugated polymer, the n-type compound, and the n-type fullerene, the organic semiconductor ink preferably contains an additive for the purpose of stabilizing the bulk heterostructure. The additives include compounds that can promote stacking of the aromatic moiety of the p-type organic semiconductor and the aromatic moiety of the n-type organic semiconductor, and can also promote the formation of a bulk heterostructure between the p-type organic semiconductor and the n-type organic semiconductor, such as polycyclic aromatic compounds and 1,8-diiodooctane.

[0057] Examples of polycyclic aromatic compounds include naphthalene, anthracene, pyrene, etc. Among these, the additive is preferably a bicyclic condensed ring such as 1-chloronaphthalene. The content of additives in the organic semiconductor ink is usually 1.5% by mass or more, preferably 2.0% by mass or more, and usually 4.0% by mass or less, preferably 3.5% by mass or less.

[0058] Furthermore, the organic semiconductor ink may contain other components to the extent that the effects of the present invention are not impaired. The content of other components is usually 2.0% by mass or less based on the organic solvent.

[0059] (Example Compound) Specific examples of the compound of formula (III) are given below.

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] (device) When the organic semiconductor device is a photoelectric conversion element, the structure of the photoelectric conversion element can be, for example, that described in JP 2007-324587 A and is not particularly limited. For example, the photoelectric conversion element may have a structure in which a transparent electrode, an electron transport layer, an active layer (photoelectric conversion layer), a hole transport layer, and a metal electrode are laminated in this order on a transparent substrate, or may have a structure in which a transparent electrode, a hole transport layer, an active layer (photoelectric conversion layer), an electron transport layer, and a metal electrode are laminated in this order on a transparent substrate.

[0064] A transparent electrode is an electrode made of a material with an average transmittance of 80% or more in visible light of 450 nm or more. There are no particular limitations on the material that can be used to form a transparent electrode, but examples include tin-doped indium oxide (ITO), zinc-doped indium oxide (IZO), tungsten-doped indium oxide (IWO), zinc aluminum oxide (AZO), indium oxide (In2O3), zinc oxide (ZnO), titanium oxide (TiO2), etc.

[0065] The metal electrode is an electrode that forms a pair with the transparent electrode. The material constituting the metal electrode is not particularly limited, and examples thereof include metals such as gold, platinum, silver, aluminum, nickel, titanium, magnesium, calcium, barium, sodium, chromium, copper, and cobalt, or alloys thereof. It is preferable that the metal electrode is a transparent electrode, that is, the pair of electrodes are transparent electrodes. In this case, the metal electrode is formed from the material forming the transparent electrode, and the pair of electrodes may be formed from the same material or different materials. The thickness of the metal electrode is not particularly limited, and if transparency is desired, it is usually about 10 nm, whereas if transparency is not required, the thickness may be 40 nm or more, more preferably 100 nm or more, taking durability and the like into consideration.

[0066] There are no particular limitations on the constituent members and manufacturing methods of the electron transport layer and hole transport layer, and well-known techniques can be used. For example, members and manufacturing methods thereof described in publicly known documents such as WO 2013 / 171517, WO 2013 / 180230, or JP 2012-191194 A can be used.

[0067] When the organic semiconductor device is a photoelectric conversion element, the photoelectric conversion element is provided in an optical sensor or an image sensor as a photodetector and used. In this case, the optical sensor and the image sensor may have a known configuration. In the organic semiconductor device according to this embodiment, by forming an active layer in combination with a p-type organic semiconductor appropriate for an n-type organic semiconductor, it is possible to make the external quantum efficiency (EQE) at 700 to 1200 nm 50% or more at least for a portion of the wavelengths, more preferably 50% or more at a wavelength of 940 nm, and even more preferably 50% or more for all wavelengths from 700 to 1200 nm.

[0068] By using an organic semiconductor device (photoelectric conversion element) having such an active layer, a photodetector for detecting light with a wavelength of 700 to 1200 nm can be obtained. EXAMPLES

[0069] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples as long as the gist of the present invention is not exceeded. Note that the numbers below the compounds in the reaction formulas are the compound numbers. The compounds were identified by APCI (atmospheric pressure chemical ionization) mass spectrometry (Shimadzu LCMS-IT-TOF).

[0070] <Experimental Example 1> [ka] Compound 1 (1.05g, 4.0mmol), compound 2 (228.1mg, 2.0mmol), Pd(PPh3)2Cl2 (70.2mg, 0.1mmol), and dppb (85.3mg, 0.2mmol) were placed in a Schlenk flask and purged with nitrogen. DBU (609mg, 4.0mmol) and DMSO (10mL) were added to the flask and heated at 80℃ for 4 hours. After cooling to room temperature, saturated ammonium chloride water (15mL) was added and extracted with ether (50mL x 2 times). The organic layer was washed with saturated saline (50mL), dried over sodium sulfate, and filtered. The organic layer was concentrated under reduced pressure, and the resulting crude product was purified by silica gel column chromatography (developing solvent: 10% ethyl acetate / hexane), obtaining compound 3 in 69% yield. MS(APCI+)294.1

[0071] <Experimental Example 2> [ka] A THF solution of phenylmagnesium bromide (11.0 mL, 9.0 mmol) was placed in a Schlenk flask and cooled to 0°C. Compound 3 (588.6 mg, 2.0 mmol) dissolved in THF (2 mL) was added dropwise over 5 minutes, and the mixture was then warmed to room temperature and stirred for 12 hours. The reaction solution was poured into ice water and extracted with ethyl acetate (15 mL x 2). The organic layer was dried over sodium sulfate and filtered. The organic layer was concentrated under reduced pressure, and the resulting crude product was dissolved in ethyl acetate / hexane and recrystallized to obtain compound 4 in 83% yield. MS(APCI+)545.2

[0072] <Experimental Example 3> [ka] Suspension of compound 4 (545.6 mg, 1.0 mmol) in methanol (10 mL) After adding CAN (219.3 mg, 0.4 mmol) to the reaction solution, the temperature was raised to 50° C. and the mixture was stirred for 12 hours. After cooling to room temperature, the reaction solution was filtered and the precipitate was washed by suspending in methanol to obtain compound 5 in a 90% yield. MS(APCI+)570.3

[0073] <Example 1> [ka] LiCl (25.4 mg, 0.60 mmol) was added to a Schlenk flask, and after drying by heating, FeCl2 (5.2 mg, 0.04 mmol), PPh3 (21.0 mg, 0.08 mmol), Mg powder (14.6 mg, 0.60 mmol), and compound 5 (114.1 mg, 0.20 mmol) were added to the mixture under a nitrogen stream. THF (0.4 mL) was added to the mixture, and the mixture was stirred at room temperature for 7 hours, after which 1,2-dichloropropane (39 μL, 0.40 mmol) was slowly added and the mixture was further stirred at room temperature for 12 hours. The reaction solution was diluted with chloroform (30 mL), the organic layer was washed with 1 M hydrochloric acid (15 mL), the organic layer was dried over sodium sulfate, and then filtered. The organic layer was concentrated under reduced pressure, and the obtained crude product was dissolved in chloroform-methanol and recrystallized to obtain the compound of Example 1 in a yield of 92%. MS(APCI+)508.7

[0074] <Experimental Example 4> [ka] A solution of compound 6 (6.4 g, 50 mmol) in THF (50 mL) was added dropwise to LDA (105 mmol) prepared from nBuLi (1.6 M, 66 mL) and diisopropylamine (10.6 g) in THF (40 mL) at -78 ° C over 10 minutes. The mixed solution was further stirred at -78 ° C, and an ether solution (40 mL) of iodine (13.9 g, 55 mmol) was added dropwise over 10 minutes. The reaction solution was warmed to room temperature and further stirred for 1 hour, after which ether (100 mL) was added and poured into ice water (300 mL). The aqueous layer was made weakly acidic with 1 M hydrochloric acid and extracted with ethyl acetate (300 mL). These organic layers were combined, dried over sodium sulfate, and filtered. The organic layer was concentrated under reduced pressure, and the resulting crude product was recrystallized from ethanol-water to obtain compound 7 in 84% yield. MS(APCI+)253.9

[0075] <Experimental Example 5> [ka] To a solution of compound 7 (10.6 g, 41.7 mmol) in methanol (80 mL), 1 mL of concentrated sulfuric acid was added and stirred at 80°C for 14 hours. After cooling to room temperature, the mixture was poured into ice water (100 mL) and neutralized by adding sodium bicarbonate. The mixture was extracted with ether (100 mL x 2), and the organic layer was dried over sodium sulfate and filtered. The organic layer was concentrated under reduced pressure to obtain compound 8 quantitatively (yield 100%). MS(APCI+)267.9

[0076] <Experimental Example 6> [ka] Compound 8 (1.07g, 4.0mmol), compound 2 (250.9mg, 2.2mmol), Pd(PPh3)2Cl2 (140.4mg, 0.2mmol), and dppb (170.6mg, 0.4mmol) were placed in a Schlenk flask and substituted with nitrogen. DMSO (40mL) was added to this, and DBU (1.22mg, 8.0mmol) was added dropwise over 5 minutes. This reaction solution was heated at 80°C for 6 hours. After cooling to room temperature, saturated ammonium chloride water (60mL) was added and extracted with ethyl acetate (60mL x 2 times). The organic layer was washed with saturated saline (50mL), dried over sodium sulfate, and filtered. The organic layer was concentrated under reduced pressure, and the obtained crude product was purified by silica gel column chromatography (developing solvent: 10% ethyl acetate / hexane), and compound 9 was obtained in 48% yield. MS(APCI+)306.0

[0077] <Experimental Example 7> [ka] A THF solution of phenylmagnesium bromide (10.0 mL, 10 mmol) was placed in a Schlenk flask and cooled to 0°C. Compound 9 (612.7 mg, 2.0 mmol) dissolved in THF (5 mL) was added dropwise over 5 minutes, and the mixture was then warmed to room temperature and stirred for 12 hours. The reaction solution was poured into ice water and extracted with ethyl acetate (15 mL x 2). The organic layer was dried over sodium sulfate and filtered. The organic layer was concentrated under reduced pressure, and the resulting crude product was dissolved in ethyl acetate / hexane and recrystallized to obtain compound 10 in a 49% yield. MS(APCI+)554.1

[0078] <Experimental Example 8> [ka] To a suspension solution of compound 10 (443.8 mg, 0.8 mmol) in methanol (2 mL), CAN (175.4 mg, 0.32 mmol) was added, and the mixture was heated to 40° C. and stirred for 12 hours. After cooling to room temperature, the reaction solution was filtered, and the precipitate was washed by suspending in methanol to obtain compound 11 in 75% yield. MS(APCI+)582.2

[0079] <Example 2> [ka] LiCl (25.4 mg, 0.60 mmol) was added to a Schlenk flask, and after drying by heating, FeCl2 (2.6 mg, 0.02 mmol), PPh3 (10.5 mg, 0.04 mmol), Mg powder (14.6 mg, 0.60 mmol), and compound 11 (116.6 mg, 0.20 mmol) were added to the mixture under a nitrogen stream. THF (0.4 mL) was added to the mixture, and the mixture was stirred at room temperature for 7 hours, after which 1,2-dichloropropane (39 μL, 0.40 mmol) was slowly added and the mixture was further stirred at room temperature for 12 hours. The reaction solution was diluted with chloroform (20 mL), the organic layer was washed with 1 M hydrochloric acid (15 mL), the organic layer was dried over sodium sulfate, and then filtered. The organic layer was concentrated under reduced pressure, and the obtained crude product was dissolved in chloroform-methanol and recrystallized to obtain the compound of Example 2 in a yield of 93%. MS(APCI+)520.1

[0080] <Examples 3 to 9> In Examples 1 and 2, the compounds in which the substituent Ar of the compounds in Examples 1 and 2 shown in the structure column in Table 1 was changed to the substituent shown in the substituent column in Table 1, and the compounds in which the aromatic rings of the compounds in Examples 1 and 2 were increased were synthesized.

[0081] [Table 1]

Claims

1. An aromatic polycyclic fused ring compound represented by the following formula (II)'. 【Chemistry 1】 (In formula (II)', R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; Ar 1 and Ar 2 is a thiophene ring, and n is an integer of 0 or more.

2. An organic semiconductor device comprising an active layer containing a p-type conjugated polymer and an n-type compound represented by the following general formula (III): 【Chemistry 2】 (In formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 are each independently selected from an optionally substituted alkyl group and an optionally substituted aromatic ring group; 1 , X 2 each independently represents a halogen atom, p and q each independently represent an integer from 0 to 4, r and s each independently represent 0 or 1, and n represents an integer of 0 or more.

3. 3. The organic semiconductor device of claim 2, wherein the active layer contains at least one fullerene compound selected from the group consisting of [60]fullerene, [70]fullerene, [60]PCBM, [70]PCBM, bis[60]PCBM, bis[70]PCBM, [60]SIMEF, [70]SIMEF, [60]ICBA, [70]ICBA, [60]ICMA, and [70]ICMA.

4. 4. The organic semiconductor device according to claim 2, wherein the active layer contains a polycyclic aromatic compound or 1,8-diiodooctane.

5. The organic semiconductor device according to any one of claims 2 to 4, which is a photoelectric conversion element.

6. 6. The organic semiconductor device according to claim 2, which has an external quantum efficiency (EQE) of 50% or more when irradiated with light having a wavelength of 940 nm.

7. 1. An organic semiconductor ink comprising: a p-type conjugated polymer; an n-type compound represented by the following general formula (III); at least one fullerene compound selected from the group consisting of [60]fullerene, [70]fullerene, [60]PCBM, [70]PCBM, bis[60]PCBM, bis[70]PCBM, [60]SIMEF, [70]SIMEF, [60]ICBA, [70]ICBA, [60]ICMA, and [70]ICMA; and a solvent, wherein the weight ratio of the fullerene compound to the n-type compound is 2.0 or less. 【Chemistry 3】 (In formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 are each independently selected from an alkyl group which may have a substituent and an aromatic ring group which may have a substituent; X 1 and X 2 each independently represent a halogen atom; p and q each independently represent an integer from 0 to 4; r and s each independently represent 0 or 1; and n represents an integer of 0 or greater.)

8. 8. The organic semiconductor ink according to claim 7, which contains a polycyclic aromatic compound and / or 1,8-diiodooctane.

9. A photodetector using the organic semiconductor device according to any one of claims 2 to 6.

10. 10. The photodetector according to claim 9, which is used to detect light having a wavelength of 700 to 1200 nm.

Citation Information

Patent Citations

  • INDACENE DERIVATIVE AND METHOD OF MANUFACTURING THE SAME, AND CARBON-BRIDGED p-PHENYLENE VINYLENE DERIVATIVE AND METHOD OF MANUFACTURING THE SAME

    JP2011032197A

  • Condensed-cyclic compound and organic light-emitting element

    JP2014058516A

  • Condensed cyclic compound and organic light-emitting device including the same

    US20190173027A1