Optically absorptive anisotropic film, three-dimensional optically absorptive anisotropic film and its manufacturing method
The light-absorbing anisotropic film with dichroic dye and liquid crystal compound addresses alignment issues in polarizing films, enhancing light transmission and absorption for improved display security.
Patent Information
- Application Number
- JP2022208455
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-06-25
- Filing Date
- 2022-12-26
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2035-06-22
AI Technical Summary
Existing polarizing films have insufficient alignment orderliness, leading to inadequate light transmission from the front direction and light absorption from oblique directions, necessitating a thin, easily manufacturable film for effective prying prevention in displays.
A light-absorbing anisotropic film containing a dichroic dye and a liquid crystal compound, with specific absorbance ratios and phase configurations, including a smectic liquid crystal phase, to enhance light absorption anisotropy and alignment.
The film effectively transmits light from the front direction while absorbing light from oblique directions, providing robust prying prevention for displays.
Smart Images

Figure 0007557518000026 
Figure 0007557518000028 
Figure 0007557518000027
Abstract
Description
[Technical field]
[0001] The present invention relates to an optically absorptive anisotropic film, a three-dimensional optically absorptive anisotropic film, and a method for producing the same. [Background technology]
[0002] Patent Document 1 describes a polarizing plate having a polarizing layer with a K value defined as K=(kx-kz) / (kx-ky) of 0.25 to 0.75. (The mutually orthogonal axes in the plane of the polarizing layer are the x-axis and y-axis, and the axis orthogonal to the xy-axis plane is the z-axis, and kx, ky, and kz are the absorption coefficients in the x-axis, y-axis, and z-axis directions, respectively.) That is, the polarizing plate satisfies the relationship of kx>kz>ky and K=0.25 to 0.75, and in the polarizing plate, the dichroic dye is oriented with an inclination with respect to the film surface. Specifically, a polarizing plate was prepared containing the following liquid crystal compounds 1 and 2 and black dichroic dye S-344 manufactured by Mitsui Toatsu as a dichroic dye, and a polarizing plate including a polarizing layer having values of kx=0.111, ky=0.001, and kz=0.059 was obtained. TIFF0007557518000001.tif70110 [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-033050 A Summary of the Invention [Problem to be solved by the invention]
[0004] The above polarizing film had a problem that the orientation order of the vertical alignment was insufficient, so that the transmission of light from the front direction and the absorption of light from oblique directions were insufficient. Therefore, there was a need for a thin, easily manufactured light-absorbing anisotropic film that could provide a more effective anti-spy function to the displays of mobile phones, bank ATMs, etc. [Means for solving the problem]
[0005] The present invention includes the following inventions. [1] An optically absorptive anisotropic film containing a dichroic dye and a liquid crystalline compound, in which the optical absorbance of the film satisfies the following formulas (1), (2), and (3) when any direction in the film plane is defined as the x-axis, the direction in the film plane perpendicular to the x-axis is defined as the y-axis, and the film thickness direction perpendicular to the x-axis and y-axis is defined as the z-axis. Az>(Ax+Ay) / 2 (1) Ax(z=60) / Ax>5 (2) Ay(z=60) / Ay>5 (3) (Ax, Ay, Az, Ax(z=60) and Ay(z=60) are all absorbances at the absorption maximum wavelengths of the dichroic dyes in the optically absorptive anisotropic film, Ax represents the absorbance of linearly polarized light vibrating in the x-axis direction, Ay represents the absorbance of linearly polarized light vibrating in the y-axis direction, Az represents the absorbance of linearly polarized light vibrating in the z-axis direction, Ax (z=60) represents the absorbance of linearly polarized light oscillating in the x-axis direction when the film is rotated 60° around the y-axis, Ay (z=60) represents the absorbance of linearly polarized light oscillating in the y-axis direction when the film is rotated 60° around the x-axis. [2] The optically absorptive anisotropic film according to [1], wherein the liquid crystalline compound forms a smectic liquid crystal phase. [3] The optically absorptive anisotropic film according to [1] or [2], wherein the liquid crystalline compound forms a high-order smectic liquid crystal phase. [4] The optically absorptive anisotropic film according to any one of [1] to [3], which exhibits a Bragg peak in X-ray diffraction measurement. [5] The optically absorptive anisotropic film according to any one of [1] to [4], wherein the dichroic dye in the optically absorptive anisotropic film has a maximum absorption wavelength in the wavelength range of 500 nm to 600 nm. [6] The optically absorptive anisotropic film according to any one of [1] to [5], which satisfies formulas (4) and (5). Ax(z=60) / Ax>10 (4) Ay(z=60) / Ay>10 (5) [7] The optically absorptive anisotropic film according to any one of [1] to [6], which contains at least three kinds of dichroic dyes having different maximum absorption wavelengths. [8] The optically absorptive anisotropic film according to any one of [1] to [7], wherein the optically absorptive anisotropic film has a thickness of 5 μm or less. [9] An optical film comprising the optically absorptive anisotropic film according to any one of [1] to [8] and a substrate.
[10] The optical film according to [9], which does not include an alignment film between the substrate and the light absorbing anisotropic film.
[11] The method for producing an optical film according to [9] or
[10] , comprising carrying out the following steps (1) to (4) in this order: (1) A step of applying a composition containing a liquid crystal compound, a dichroic dye, and a solvent onto a substrate to form a coating film. (2) A process of removing the solvent from the coating film to form a dry film. (3) A step of cooling the dried film to develop a liquid crystal phase. (4) A step of curing the liquid crystal compound by irradiating it with active energy rays.
[12] The method according to
[11] , in which a long film is used as the substrate and an optical film is continuously produced.
[13] A three-dimensional optically absorptive anisotropic film obtained by laminating the optically absorptive anisotropic film according to any one of [1] to [8] and a horizontal polarizing film, wherein the three-dimensional optically absorptive anisotropic film satisfies the following formula (4) when the absorption axis of the horizontal polarizing film is the x' axis, the transmission axis of the horizontal polarizing film is the y' axis, and the axis perpendicular to the x' axis and the y' axis is the z' axis. Ax'>Az'>Ay' (6) (Ax', Ay', and Az' are all absorbances at the absorption maximum wavelengths of the dichroic dyes in the optically absorptive anisotropic film, Ax' represents the absorbance of linearly polarized light vibrating in the x' direction, Ay' represents the absorbance of linearly polarized light vibrating in the y' direction, Az' represents the absorbance of linearly polarized light vibrating in the z' direction.)
[14] The three-dimensional optically absorptive anisotropic film according to
[13] , wherein the horizontal polarizing film contains polyvinyl alcohol and a dichroic dye.
[15] The three-dimensional optically absorptive anisotropic film according to
[13] , wherein the horizontal polarizing film contains a dichroic dye and a liquid crystalline compound, or contains a dichroic dye having liquid crystal properties.
[16] The three-dimensional optically absorptive anisotropic film according to any one of
[13] to
[15] , wherein the optically absorptive anisotropic film is laminated on a horizontal polarizing film via a pressure-sensitive adhesive or bonding agent. Effect of the Invention
[0006] According to the present invention, it is possible to obtain a thin, easily manufactured light absorbing anisotropic film that provides a function of adequately preventing peeping on the displays of mobile phones, bank ATMs, and the like. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a perspective view of the present optically absorptive anisotropic film. [Diagram 2] 1 is a schematic diagram of a method for producing an optically absorptive anisotropic film. [Diagram 3] FIG. 2 is a perspective view of an example of a three-dimensional optically absorptive anisotropic film. [Figure 4] FIG. 1 is a perspective view of a liquid crystal display device having a three-dimensional optically absorptive anisotropic film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Light-absorbing anisotropic film> The optically absorptive anisotropic film is a film containing a dichroic dye. The optically absorptive anisotropic film of the present invention contains a dichroic dye and a liquid crystal compound.
[0009] The optically absorptive anisotropic film satisfies all of the following formulas (1), (2), and (3) when any direction in the film plane is defined as the x-axis, the direction perpendicular to the x-axis in the film plane is defined as the y-axis, and the film thickness direction perpendicular to the x-axis and y-axis is defined as the z-axis (see FIG. 1). Az>(Ax+Ay) / 2 (1) Ax(z=60) / Ax>5 (2) Ay(z=60) / Ay>5 (3) Here, Ax, Ay, Az, Ax(z=60) and Ay(z=60) are all absorbances at the maximum absorption wavelengths of the dichroic dyes in the optically absorptive anisotropic film. Ax represents the absorbance of linearly polarized light vibrating in the x-axis direction. Ax can be measured by injecting linearly polarized light vibrating in the x-axis direction from the z-axis direction toward the film surface. Ay represents the absorbance of linearly polarized light vibrating in the y-axis direction. Ay can be measured by injecting linearly polarized light vibrating in the y-axis direction from the z-axis direction toward the film surface. Az represents the absorbance of linearly polarized light vibrating in the z-axis direction. Az can be measured, for example, by injecting linearly polarized light vibrating in the z-axis direction from the xy plane direction toward the film side surface, that is, perpendicular to the side surface (thickness direction) when the film is an xy plane. Ax (z = 60) represents the absorbance of linearly polarized light vibrating in the x-axis direction when the film is rotated 60° around the y-axis as the rotation axis. Ax (z = 60) can be measured by injecting the same linearly polarized light as that used to measure Ax, with the film rotated 60° around the y-axis as the rotation axis. Here, the film is rotated by rotating the film in the state where Ax was measured by 60° in the incident direction of linearly polarized light with the y-axis as the rotation axis. Ay(z=60) represents the absorbance of linearly polarized light vibrating in the y-axis direction when the film is rotated by 60° with the x-axis as the rotation axis. Ay(z=60) can be measured by rotating the film by 60° with the x-axis as the rotation axis and then incidenting the same linearly polarized light as that used to measure Ay. Here, the film is rotated by rotating the film in the state where Ay was measured by 60° in the incident direction of linearly polarized light with the x-axis as the rotation axis.
[0010] The absorbance in the z direction in equation (1) is difficult to measure because light is incident from the side of the film. Therefore, when the angle between the vibration plane of the linearly polarized light (measurement light) and the xy plane of the film is 90°, the absorbance in the Az direction can be estimated by measuring while tilting the xy plane of the film by 30° and 60° to the incident direction of the linearly polarized light with respect to this vibration plane. Specifically, it can be estimated by the following methods. With the film rotated by 30° and 60° about the y-axis as the rotation axis, Ax(z = 30) and Ax(z = 60) are measured by incident linearly polarized light identical to the linearly polarized light for which Ax was measured. Similarly, with the film rotated by 30° and 60° about the x-axis as the rotation axis, Ay(z = 30) and Ay(z = 60) are measured by incident linearly polarized light identical to the linearly polarized light for which Ay was measured. At this time, if Ax(z = 30) < Ax(z = 60) and Ay(z = 30) = Ay(z = 60), then Ax(z = 30) < Ax(z = 60) < Ax(z = 90) = Az, and if Ay(z = 30) < Ay(z = 60) and Ax(z = 30) = Ax(z = 60), then Ay(z = 30) < Ay(z = 60) < Ay(z = 90) = Az. Thus, it can be said that equation (1) is necessarily satisfied.
[0011] In particular, when there is no absorption anisotropy in the x - y plane, that is, when Ax and Ay are equal, since Ax(z = 30) = Ay(z = 30) and Ax(z = 60) = Ay(z = 60), Ax(z = 30) and Ay(z = 30) can be denoted as A(z = 30), and Ax(z = 60) and Ay(z = 60) can be denoted as A(z = 60). That is, if A(z = 30) < A(z = 60), the relationship A(z = 30) < A(z = 60) < A(z = 90) = Az is satisfied. Further, if A(z = 30) > (Ax + Ay) / 2, it can be said that Az necessarily satisfies equation (1).
[0012] The light absorption anisotropic film of the present invention satisfies the above equations (2) and (3). Ax(z = 60) / Ax and Ay(z = 60) / Ay mean that the larger the numerical value, the more excellent the light absorption anisotropy is shown. These numerical values may be, for example, 50 or less, or may be 30 or less. Also, the light absorption anisotropic film of the present invention preferably satisfies equations (4) and (5). Ax(z = 60) / Ax > 10 (4) Ay(z = 60) / Ay > 10 (5)
[0013] When the optically absorptive anisotropic film satisfies the formulas (1), (2), and (3), the dichroic dye can be said to have excellent absorption anisotropy, i.e., excellent polarization performance. This excellent characteristic allows the film to effectively transmit light from the front direction and effectively absorb light from oblique directions.
[0014] The thickness of the optically absorptive anisotropic film is preferably 0.1 to 10 μm, more preferably 1 to 5 μm. If the thickness of the optically absorptive anisotropic film is less than 0.1 μm, the absorption of light from oblique directions is weak, and good anti-sneaking properties cannot be obtained. If the thickness is 10 μm or more, the orientation of the dichroic dye is disturbed, resulting in a problem of reduced transmission properties in the front direction.
[0015] <Dichroic dye> A dichroic dye is a dye that has different absorbance in the long axis direction of the molecule and absorbance in the short axis direction.
[0016] The dichroic dye preferably has an absorption maximum wavelength (λMAX) in the present optically absorptive anisotropic film in the range of 300 to 700 nm, and more preferably has an absorption maximum wavelength in the range of 500 to 600 nm. By having an absorption maximum wavelength in the range of 500 to 600 nm, where human luminosity is high, it is possible to more sufficiently prevent peeping. In other words, by using a dichroic dye having an absorption maximum at a wavelength with high luminosity, it is possible to reduce the amount of dichroic dye used and to make the optically absorptive anisotropic film thinner. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, among which bisazo dyes and trisazo dyes are preferred. The dichroic dyes may be used alone or in combination, but when polarization characteristics are required over the entire visible light range, it is preferred to combine three or more dichroic dyes, and more preferred to combine three or more azo dyes. When a plurality of dichroic dyes are combined, it is preferable to include at least one dye having a maximum absorption wavelength in the wavelength range of 500nm to 600nm in the present light absorption anisotropic film. When two dichroic dyes are combined, it is preferable to further include one having a maximum absorption wavelength in the range of 350nm to 499nm or 601nm to 750nm, and when three dichroic dyes are combined, it is preferable to include dichroic dyes having a maximum absorption wavelength in the range of 350nm to 499nm, 500nm to 600nm, and 601nm to 750nm, respectively. By combining in this way, it is possible to more sufficiently prevent peeping.
[0017] An example of the azo dye is a compound represented by formula (2) (hereinafter sometimes referred to as "compound (2)"). A 1 (-N=NA 2 ) p -N=NA 3 (2) [In formula (2), A 1 and A 3 A each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents an optionally substituted 1,4-phenylene group, an optionally substituted naphthalene-1,4-diyl group, or an optionally substituted divalent heterocyclic group. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of A 2 may be the same or different.]
[0018] Examples of the monovalent heterocyclic group include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, and benzoxazole. Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from the above heterocyclic compounds.
[0019] A 1 and A 3Phenyl, naphthyl and monovalent heterocyclic groups in the above formula, and A 2 Examples of the substituent that the 1,4-phenylene group, naphthalene-1,4-diyl group, and divalent heterocyclic group in the formula (I) may optionally have include alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, and butyl groups; alkoxy groups having 1 to 4 carbon atoms, such as methoxy, ethoxy, and butoxy groups; fluorinated alkyl groups having 1 to 4 carbon atoms, such as trifluoromethyl groups; cyano groups; nitro groups; halogen atoms, such as chlorine atoms and fluorine atoms; and substituted or unsubstituted amino groups, such as amino groups, diethylamino groups, and pyrrolidino groups (the substituted amino group refers to an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. The unsubstituted amino group is -NH2. ) are included. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, and a hexyl group. Examples of the alkanediyl group having 2 to 8 carbon atoms include an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, and an octane-1,8-diyl group.
[0020] Among the compounds (2), the compounds represented by the following formulas (2-1) to (2-6) are preferred.
[0021] TIFF0007557518000002.tif83109
[0022] TIFF0007557518000003.tif74127 [In formulas (2-1) to (2-6), B 1 ~B 20 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]
[0023] The anthraquinone dye is preferably a compound represented by formula (2-7). TIFF0007557518000004.tif3179 [In formula (2-7), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0024] The oxazine dye is preferably a compound represented by formula (2-8). TIFF0007557518000005.tif3177 [In formula (2-8), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0025] The acridine dye is preferably a compound represented by formula (2-9). TIFF0007557518000006.tif3171 [In formula (2-9), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0026] R in formula (2-7), formula (2-8) and formula (2-9) x Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, and a butyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.
[0027] As the cyanine dye, the compounds represented by formula (2-10) and formula (2-11) are preferred. TIFF0007557518000007.tif1555 [In formula (2-10), D 1 and D. 2 each independently represents a group represented by any one of formulas (2-10a) to (2-10d). TIFF0007557518000008.tif27128 n5 represents an integer from 1 to 3.
[0028] TIFF0007557518000009.tif1856 [In formula (2-11), D 3 and D. 4 each independently represents a group represented by any one of formulas (2-11a) to (2-11h). TIFF0007557518000010.tif64110 n6 represents an integer from 1 to 3.
[0029] From the viewpoint of improving the alignment of the dichroic dye, the content of the dichroic dye in the optically absorptive anisotropic film is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, even more preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the solid content of the optically absorptive anisotropic composition. If the content of the dichroic dye is within this range, it is preferable because the liquid crystal alignment of the liquid crystal compound is not easily disturbed.
[0030] <Base material> The present optically absorptive anisotropic film can be formed by a method such as coating a composition containing a dichroic dye (hereinafter, sometimes referred to as the present optically absorptive anisotropic composition) on a substrate. The substrate may be a glass substrate or a resin substrate, but is preferably a resin substrate. In the case where the resin substrate is transferred and not peeled off, a transparent resin substrate is preferable. The transparent resin substrate means a substrate having a light-transmitting property capable of transmitting light, particularly visible light, and the light-transmitting property means a property that the luminosity-corrected transmittance for light rays having a wavelength of 380 nm to 780 nm is 80% or more.
[0031] Examples of the resin constituting the substrate include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin-based resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyether ketone; polyphenylene sulfide; and polyphenylene oxide. Preferred are cellulose esters, cyclic olefin-based resins, polycarbonate, polyethersulfone, polyethylene terephthalate, and polymethacrylic acid esters.
[0032] Cellulose ester is a material in which at least a part of the hydroxyl groups contained in cellulose is esterified, and can be obtained from the market. In addition, substrates containing cellulose esters can also be obtained from the market. Examples of commercially available substrates containing cellulose esters include Fujitac (registered trademark) film (FUJIFILM Corporation), KC8UX2M (KONICA MINOLTA OPT, Inc.), KC8UY (KONICA MINOLTA OPT, Inc.), and KC4UY (KONICA MINOLTA OPT, Inc.).
[0033] The cyclic olefin resin includes a polymer of a cyclic olefin such as norbornene or a polycyclic norbornene monomer, or a copolymer thereof. The cyclic olefin resin may include a ring-open structure, or may be a hydrogenated cyclic olefin resin including a ring-open structure. The cyclic olefin resin may include a structural unit derived from a chain olefin and a vinylated aromatic compound, as long as the transparency is not significantly impaired and the moisture absorption is not significantly increased. The cyclic olefin resin may have a polar group introduced into its molecule. Examples of the linear olefin include ethylene and propylene, and examples of the vinylated aromatic compounds include styrene, α-methylstyrene, and alkyl-substituted styrenes.
[0034] When the cyclic olefin resin is a copolymer of a cyclic olefin and a chain olefin or a vinylated aromatic compound, the content of structural units derived from the cyclic olefin is usually 50 mol % or less, and preferably 15 to 50 mol %, based on the total structural units of the copolymer. When the cyclic olefin resin is a terpolymer of a cyclic olefin, a chain olefin, and a vinylated aromatic compound, the content of the structural unit derived from the chain olefin is usually 5-80 mol% based on the total structural units of the copolymer, and the content of the structural unit derived from the vinylated aromatic compound is usually 5-80 mol% based on the total structural units of the copolymer. Such a terpolymer has the advantage that the amount of expensive cyclic olefin used can be relatively reduced.
[0035] Cyclic olefin resins are commercially available. Examples of commercially available cyclic olefin resins include Topas (registered trademark) (Ticona, Germany), Arton (registered trademark) (JSR Corporation), ZEONOR (registered trademark) (ZEON Corporation), ZEONEX (registered trademark) (ZEON Corporation), and APEL (registered trademark) (Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a substrate. Examples of substrates containing commercially available cyclic olefin resins include S-Cina (registered trademark) (Sekisui Chemical Co., Ltd.), SCA40 (registered trademark) (Sekisui Chemical Co., Ltd.), ZEONOR Film (registered trademark) (Optes Co., Ltd.), and Arton Film (registered trademark) (JSR Corporation).
[0036] The substrate may be subjected to a surface treatment. Examples of the surface treatment method include a method of treating the substrate surface with corona or plasma under an atmosphere from vacuum to atmospheric pressure, a method of laser treating the substrate surface, a method of ozone treating the substrate surface, a method of saponifying the substrate surface, a method of flame treating the substrate surface, a method of applying a coupling agent to the substrate surface, a method of primer treating the substrate surface, and a graft polymerization method in which reactive monomers or reactive polymers are attached to the substrate surface and then reacted by irradiating radiation, plasma or ultraviolet light. Among these, a method of corona or plasma treating the substrate surface under an atmosphere from vacuum to atmospheric pressure is preferred.
[0037] Methods for performing surface treatment of a substrate with corona or plasma include a method for placing the substrate between opposing electrodes under pressure close to atmospheric pressure and generating corona or plasma to perform surface treatment of the substrate, a method for flowing a gas between opposing electrodes, converting the gas into plasma between the electrodes, and spraying the plasmatized gas onto the substrate, and a method for generating glow discharge plasma under low pressure conditions to perform surface treatment of the substrate.
[0038] Among these, a method of placing a substrate between opposing electrodes under a pressure close to atmospheric pressure, generating a corona or plasma to perform surface treatment of the substrate, or a method of flowing a gas between opposing electrodes, converting the gas into plasma between the electrodes, and spraying the plasma gas onto the substrate is preferred. Such surface treatment using corona or plasma is usually performed using a commercially available surface treatment device.
[0039] The substrate may have a protective film on the surface opposite to the surface on which the optically absorptive anisotropic composition is applied. Examples of the protective film include films of polyethylene, polyethylene terephthalate, polycarbonate, polyolefin, and the like, as well as films further having an adhesive layer thereon. Among them, polyethylene terephthalate is preferred because it has small thermal deformation during drying. By having a protective film on the surface opposite to the surface on which the optically absorptive anisotropic composition is applied, it is possible to suppress the shaking of the film during transport of the substrate and slight vibration of the coating surface, and improve the uniformity of the coating film.
[0040] The thickness of the substrate is preferably thin in terms of the weight that allows practical handling, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the substrate is usually 5 to 300 μm, and preferably 20 to 200 μm.
[0041] The length of the substrate in the longitudinal direction is usually 10 to 3000 m, preferably 100 to 2000 m, and the length of the substrate in the lateral direction is usually 0.1 to 5 m, preferably 0.2 to 2 m.
[0042] <Liquid crystal compounds> The optically absorptive anisotropic film of the present invention is a liquid crystal cured film containing a dichroic dye and a liquid crystal compound. The liquid crystal compound contained in the present optically absorptive anisotropic film is preferably a polymerizable liquid crystal compound. The polymerizable liquid crystal compound is a compound that has a polymerizable group and has liquid crystal properties. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred. The liquid crystal compound may be a thermotropic liquid crystal or a lyotropic liquid crystal, and the phase order structure in the thermotropic liquid crystal may be a nematic liquid crystal or a smectic liquid crystal. A compound that forms a smectic liquid crystal phase is preferable, and a compound that forms a high-order smectic liquid crystal phase such as a smectic B phase is more preferable. When the liquid crystal phase formed by the liquid crystal compound is a high-order smectic phase, a light absorption anisotropic film with a higher degree of orientation order can be produced, and by increasing the degree of orientation order, the values of Ax(z=60) / Ax and Ay(z=60) / Ay tend to be higher.
[0043] As the polymerizable liquid crystal compound, a smectic liquid crystal compound is preferred in that a higher polarization performance can be obtained, and a higher-order smectic liquid crystal compound is more preferred. Among them, a higher-order smectic liquid crystal compound that forms a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferred, and a higher-order smectic liquid crystal compound that forms a smectic B phase, a smectic F phase, or a smectic I phase is more preferred. When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these higher-order smectic phases, a liquid crystal cured film with a higher degree of orientation order can be produced, and high polarization performance can be obtained. In addition, such a liquid crystal cured film with a high degree of orientation order is one that can obtain a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystal phase in X-ray diffraction measurement. The Bragg peak is a peak derived from the periodic structure of molecular orientation, and a film having a periodic interval of 3.0 to 6.0 Å can be obtained. Specific examples of such smectic liquid crystal compounds include a compound represented by the following formula (1) (hereinafter, sometimes referred to as compound (1)). The polymerizable liquid crystal compounds may be used alone or in combination.
[0044] U 1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (1) [In formula (1), X 1 , X 2 and X 3 each independently represents an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group, provided that X 1 , X 2 and X 3At least one of the groups is a 1,4-phenylene group which may have a substituent. -CH2- constituting the cyclohexane-1,4-diyl group may be replaced by -O-, -S- or NR-. R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group. Y 1 and Y 2 are each independently -CH2CH2-, -CH2O-, -COO-, -OCOO-, a single bond, -N=N-, -CR a =CR b -, -C≡C- or CR a =N-. R a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. U 1 represents a hydrogen atom or a polymerizable group. U 2 represents a polymerizable group. W 1 and W 2 represent, independently of one another, a single bond, -O-, -S-, -COO- or -OCOO-. V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -S- or NH-.]
[0045] In compound (1), X 1 , X 2 and X 3 At least one of these is preferably a 1,4-phenylene group which may have a substituent. The 1,4-phenylene group which may have a substituent is preferably unsubstituted. The cyclohexane-1,4-diyl group which may have a substituent is preferably a trans-cyclohexane-1,4-diyl group which may have a substituent, and the trans-cyclohexane-1,4-diyl group which may have a substituent is preferably unsubstituted.
[0046] Examples of the substituent that the 1,4-phenylene group which may have a substituent or the cyclohexane-1,4-diyl group which may have a substituent include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom.
[0047] Y 1 is preferably -CH2CH2-, -COO- or a single bond, and Y 2 is preferably -CH2CH2- or CH2O-.
[0048] U 2 is a polymerizable group. 1 is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group. 1 and U 2 Preferably, both of and are polymerizable groups, and more preferably, both of and are photopolymerizable groups. A polymerizable liquid crystal compound having a photopolymerizable group is advantageous in that it can be polymerized under lower temperature conditions.
[0049] U 1 and U 2 The polymerizable groups represented by may be different from each other, but are preferably the same. Examples of the polymerizable group include vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, acryloyloxy group, methacryloyloxy group, oxiranyl group, and oxetanyl group. Among them, acryloyloxy group, methacryloyloxy group, vinyloxy group, oxiranyl group, and oxetanyl group are preferred, and acryloyloxy group is more preferred.
[0050] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group.1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms. Examples of the substituent that the optionally substituted alkanediyl group having 1 to 20 carbon atoms may have include a cyano group and a halogen atom such as a chlorine atom or a fluorine atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted, linear alkanediyl group.
[0051] Preferably, W 1 and W 2 are each independently a single bond or O-.
[0052] Specific examples of compound (1) include compounds represented by formulas (1-1) to (1-23). When compound (1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans type.
[0053] TIFF0007557518000011.tif155139
[0054] TIFF0007557518000012.tif91136
[0055] TIFF0007557518000013.tif89144
[0056] TIFF0007557518000014.tif84144
[0057] Among the exemplified compounds (1), at least one selected from the group consisting of compounds represented by formulas (1-2), (1-3), (1-4), (1-6), (1-7), (1-8), (1-13), (1-14) and (1-15) is preferred.
[0058] The exemplified compound (1) can be used alone or in combination in the liquid crystal cured film. In addition, when two or more kinds of polymerizable liquid crystal compounds are combined, it is preferable that at least one of them is compound (1), and more preferable that two or more kinds are compound (1). By combining them, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. The mixing ratio when combining two kinds of polymerizable liquid crystal compounds is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50. When combining two kinds of polymerizable liquid crystal compounds and only one of them is compound (1), it is preferable that compound (1) is blended so that it is a high proportion in the above mixing ratio.
[0059] The polymerizable liquid crystal compound can be produced by a known method, for example, as described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.
[0060] The content ratio of the liquid crystal compound in the optically absorptive anisotropic film is usually 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 80 to 94 parts by mass, and even more preferably 80 to 90 parts by mass, relative to 100 parts by mass of the optically absorptive anisotropic film, from the viewpoint of increasing the alignment of the liquid crystal compound. The content ratio of the liquid crystal compound in the optically absorptive anisotropic film can be calculated as the ratio of the liquid crystal compound to 100 parts by mass of the solid content of the optically absorptive anisotropic composition forming the optically absorptive anisotropic film.
[0061] <Polymerization initiator> The optically absorptive anisotropic composition may contain a polymerization initiator. The polymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound, etc. As the polymerization initiator, a photopolymerization initiator that generates active radicals by the action of light is preferable.
[0062] Examples of the polymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, and a sulfonium salt.
[0063] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0064] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0065] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0066] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0067] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl]-1,3,5-triazine. 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.
[0068] The polymerization initiator may be commercially available. Examples of commercially available polymerization initiators include Irgacure (registered trademark) 907, 184, 651, 819, 250, and 369 (BASF); Seikuol (registered trademark) BZ, Z, and BEE (Seiko Chemical Co., Ltd.); Kayacure (registered trademark) BP100 and UVI-6992 (Nippon Kayaku Co., Ltd.); Adeka Optomer SP-152 and SP-170 (ADEKA Co., Ltd.); TAZ-A and TAZ-PP (DKSH Japan Co., Ltd.); and TAZ-104 (Sanwa Chemical Co., Ltd.).
[0069] The content of the polymerization initiator is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound, from the viewpoint of preventing the alignment of the polymerizable liquid crystal compound from being disturbed.
[0070] <Leveling agent> The optically absorptive anisotropic film may contain a leveling agent. The leveling agent has a function of adjusting the fluidity of the optically absorptive anisotropic composition and making the optically absorptive anisotropic film flatter, and can be, for example, a surfactant. Preferred leveling agents include a leveling agent mainly composed of a polyacrylate compound and a leveling agent mainly composed of a fluorine atom-containing compound.
[0071] Examples of leveling agents containing a polyacrylate compound as a main component include BYK-350, BYK-352, BYK-353, BYK-354, BYK-355, BYK-358N, BYK-361N, BYK-380, BYK-381, and BYK-392 (BYK Chemie).
[0072] Examples of leveling agents containing a fluorine atom-containing compound as a main component include Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-471, F-477, F-479, F-482, and F-483 (DIC Corporation); Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, and SA-100 (AGC Seimi Chemical Co., Ltd.); E1830 and E5844 (Daikin Industries, Ltd.); F-top EF301, EF303, EF351, and EF352 (Mitsubishi Materials Electronic Chemicals Co., Ltd.).
[0073] The content of the leveling agent in the optically absorptive anisotropic film is usually from 0.01 to 5 parts by mass, and preferably from 0.1 to 3 parts by mass, based on 100 parts by mass of the liquid crystal compound. When the content of the leveling agent is within the above range, the obtained liquid crystal cured film tends to be smoother, which is preferable. When the content of the leveling agent relative to the liquid crystal compound exceeds the above range, the obtained liquid crystal cured film tends to be uneven or tends to be aligned in the horizontal direction, which is not preferable. The light absorption anisotropic film may contain two or more types of leveling agents.
[0074] <Solvent> The optically absorptive anisotropic composition used in forming the optically absorptive anisotropic film may contain a solvent. When the liquid crystal composition contains a liquid crystal compound, the solvent is preferably one that can completely dissolve the liquid crystal compound. When the liquid crystal compound is a polymerizable liquid crystal compound, the solvent is preferably one that is inactive to the polymerization reaction.
[0075] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone or propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorine-containing solvents such as chloroform and chlorobenzene. These solvents may be used alone or in combination.
[0076] The content of the solvent is preferably 50 to 98% by mass based on the total amount of the optically absorptive anisotropic composition, in other words, the proportion of the optically absorptive anisotropic film components is preferably 2 to 50% by mass based on the total amount of the optically absorptive anisotropic composition. When the solid content is 50% by mass or less based on the total amount of the optically absorptive anisotropic composition, the viscosity of the optically absorptive anisotropic composition is low, and therefore the thickness of the liquid crystal cured film becomes substantially uniform, and the liquid crystal cured film tends to be less prone to unevenness. In addition, such a solid content can be determined in consideration of the thickness of the liquid crystal cured film to be produced.
[0077] <Alignment film> An optical film having an optically absorptive anisotropic film and a substrate may include an alignment film between the substrate and the optically absorptive anisotropic film. The alignment film in the present invention has an alignment regulating force for aligning a dichroic dye or a liquid crystal compound in a direction perpendicular to the substrate. The alignment film is preferably one having solvent resistance such that the optically absorptive anisotropic composition is not dissolved by coating, etc., and also has heat resistance in a heat treatment for removing the solvent and for orienting the liquid crystal compound. Examples of such an alignment film include an alignment film containing an orienting polymer, a photoalignment film, etc.
[0078] <Alignment film containing alignment polymer> Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. Two or more oriented polymers may be used in combination.
[0079] An alignment film containing an alignment polymer is usually formed on the surface of a substrate by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an alignment polymer composition) to the substrate and then removing the solvent, or by applying the alignment polymer composition to the substrate, removing the solvent, and rubbing the substrate (rubbing method).
[0080] Examples of the solvent include water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, and other alcohol solvents, ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, ethyl lactate, and other ester solvents, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, methyl isobutyl ketone, and other ketone solvents, pentane, hexane, heptane, and other aliphatic hydrocarbon solvents, toluene, xylene, and other aromatic hydrocarbon solvents, acetonitrile, and other nitrile solvents, tetrahydrofuran, dimethoxyethane, and other ether solvents, and chloroform, chlorobenzene, and other chlorinated hydrocarbon solvents. These solvents may be used alone or in combination of two or more.
[0081] The concentration of the orienting polymer in the orienting polymer composition may be within a range in which the orienting polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20 mass % in terms of solid content relative to the solution, and more preferably about 0.1 to 10 mass %.
[0082] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0083] The method of applying the oriented polymer composition to the substrate includes known methods such as spin coating, extrusion, gravure coating, die coating, slit coating, bar coating, applicator, and other application methods, and flexographic printing methods. When the present optically absorptive anisotropic film is produced by a roll-to-roll continuous production method described below, the application method generally employs a printing method such as gravure coating, die coating, or flexographic printing.
[0084] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0085] In order to impart an alignment control force to the alignment film, rubbing is performed as necessary (rubbing method). By selecting the rubbing direction, the direction of the alignment control force can be arbitrarily controlled.
[0086] An example of a method for imparting an orientation control force by a rubbing method is to bring an oriented polymer film formed on the surface of a substrate by applying an oriented polymer composition to the substrate and annealing the composition into contact with a rotating rubbing roll wrapped with a rubbing cloth.
[0087] <Photo-alignment film> A photo-alignment film is usually formed on the surface of a substrate by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter, sometimes referred to as a "photo-alignment film-forming composition") to the substrate and irradiating the substrate with light (preferably polarized UV). Photo-alignment films are more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated light.
[0088] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that are the origin of liquid crystal alignment ability, such as molecular alignment induction caused by light irradiation or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond) and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0089] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazole groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0090] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.
[0091] The solvent contained in the composition for forming a photo-alignment film may be the same as the solvent contained in the above-mentioned alignable polymer composition, and may be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.
[0092] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the intended photo-alignment film, but is preferably at least 0.2% by mass, and more preferably in the range of 0.3 to 10% by mass. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.
[0093] The method for applying the composition for forming a photo-alignment film to a substrate may be the same as the method for applying the alignable polymer composition to a substrate. The method for removing the solvent from the applied composition for forming a photo-alignment film may be the same as the method for removing the solvent from the alignable polymer composition.
[0094] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The polarized UV light can be irradiated by passing the light from the light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as Glan-Thompson or Glan-Taylor, or a wire grid type polarizer can be used.
[0095] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0096] The thickness of the alignment film is usually 10 nm to 10,000 nm, preferably 10 nm to 1,000 nm, and more preferably 10 nm to 500 nm.
[0097] <Method of manufacturing the optical film and the light absorption anisotropic film> The optically absorptive anisotropic film is obtained by orienting the absorption axis of the dichroic dye in a direction perpendicular to the film surface. The direction of the absorption axis of the dichroic dye in a host-guest type optically absorptive anisotropic film such as the optically absorptive anisotropic film is usually controlled by the direction in which the liquid crystal compound is oriented. By orienting the molecular long axis of the liquid crystal compound in a direction perpendicular to the film surface, the absorption axis of the dichroic dye can usually be oriented in a direction perpendicular to the film surface. The orientation direction of the liquid crystal compound is controlled by the properties of the substrate or orientation film on which the composition containing the liquid crystal compound, the dichroic dye, and the solvent is applied, as well as the properties of the liquid crystal compound. That is, the optically absorptive anisotropic film can be obtained by using a substrate or orientation film having an orientation control force that aligns in a direction perpendicular to the film surface (vertical direction), or by using a liquid crystal compound that is easily oriented in a vertical direction. A liquid crystal compound having a smectic liquid crystal phase tends to be easily oriented vertically. An optically absorptive anisotropic film obtained by orienting the absorption axis of a dichroic dye in a direction perpendicular to the film surface satisfies the above formula (1), but may not satisfy the above formulas (2) and (3). By using a compound that forms a high-order smectic liquid crystal phase as the liquid crystal compound, an optically absorptive anisotropic film that also satisfies the above formulas (2) and (3) tends to be obtained. Specifically, the present optical film can be produced by carrying out the following steps (1) to (4) in the order described below. The optically absorptive anisotropic film can be obtained by transferring the optical film to another adherend via an adhesive or the like, and then removing the substrate. (1) A step of applying a composition containing a liquid crystal compound, a dichroic dye, and a solvent onto a substrate to form a coating film. (2) A process of removing the solvent from the coating film to form a dry film. (3) A step of cooling the dried film to cause the liquid crystal phase to appear. (4) A step of irradiating the liquid crystal compound with active energy rays to cure the liquid crystal compound. <Step (1)> Examples of a method for applying a composition (optically absorptive anisotropic composition) containing a liquid crystal compound, a dichroic dye, and a solvent to a substrate include the same methods as those exemplified as a method for applying an oriented polymer composition to a substrate.
[0098] <Step (2)> When the optically absorptive anisotropic composition contains a solvent, the solvent is usually removed from the applied optically absorptive anisotropic composition. Examples of methods for removing the solvent include natural drying, ventilation drying, heat drying, and reduced pressure drying. The dried film is preferably dried so that the remaining solvent in the optically absorptive anisotropic film is 1% by weight or less based on the total weight of the optically absorptive anisotropic film. The amount of remaining solvent can be quantified by peeling the optically absorptive anisotropic film from the substrate, weighing it, immersing the obtained optically absorptive anisotropic film in a solvent that dissolves the optically absorptive anisotropic film, such as tetrahydrofuran, irradiating it with ultrasonic waves for 10 minutes to extract the dissolved components, and then analyzing the solution by gas chromatography.
[0099] <Step (3)> The coated liquid crystal compound is usually heated to a temperature at which it transitions to a liquid crystal state or a solution state or higher, and then cooled to a temperature at which the liquid crystals are aligned, thereby forming a liquid crystal phase.
[0100] The temperature at which the applied liquid crystal compound is oriented may be determined in advance by observing the texture of a composition containing the liquid crystal compound. The removal of the solvent and the alignment of the liquid crystal may be performed simultaneously. The temperature at this time is preferably in the range of 50 to 200°C, depending on the type of the solvent to be removed and the type of the liquid crystal compound contained, and more preferably in the range of 80 to 130°C when the substrate is a resin substrate.
[0101] <Step (4)> The aligned liquid crystal compound is irradiated with active energy rays to polymerize the liquid crystal compound.
[0102] The polymerized liquid crystal compound becomes a light-absorption anisotropic film. A liquid crystal cured film containing a polymerizable liquid crystal compound polymerized while maintaining a smectic liquid crystal phase has higher polarization performance than a conventional host-guest type polarizing film, i.e., a polarizing film obtained by polymerizing a polymerizable liquid crystal compound while maintaining a nematic liquid crystal phase, and is also superior in polarization performance and strength to a film coated with only a dichroic dye or a lyotropic liquid crystal.
[0103] The light source of the active energy ray may be any light source that generates ultraviolet rays, electron beams, X-rays, etc. Preferred are light sources having an emission distribution at a wavelength of 400 nm or less, such as low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, chemical lamps, black light lamps, microwave excited mercury lamps, and metal halide lamps. It is more preferable that the active energy rays are ultraviolet rays parallel to the normal direction of the substrate.
[0104] The irradiation energy of the active energy rays is 10 to 5000 mJ / cm in the wavelength range effective for activating the polymerization initiator. 2 It is preferable to set the value so as to be within a range of 100 to 2000 mJ / cm. 2 The irradiation energy is 10 mJ / cm 2 If the temperature is too low, the liquid crystal compound tends to be insufficiently cured.
[0105] <Continuous manufacturing method of the present optical film> The present optical film is preferably continuously manufactured by a roll to roll system. With reference to FIG. 2, an example of the main part of the method for continuously manufacturing by a roll to roll system will be described. In the following description, a manufacturing method in which an alignment film is included between the substrate and the optically absorptive anisotropic film is described, but it goes without saying that the optically absorptive anisotropic film does not necessarily have to include an alignment film. In the following description, a manufacturing method in which a polymerizable liquid crystal compound is used as the liquid crystal compound is described, but the present invention is not limited to this.
[0106] The first roll 210 in which the substrate is wound around the first winding core 210A is, for example, easily available on the market. Examples of substrates available on the market in the form of such a roll include films made of cellulose ester, cyclic olefin resin, polycarbonate, polyethylene terephthalate, or polymethacrylic acid ester, among the substrates already exemplified.
[0107] Next, the substrate is unwound from the first roll 210. The method of unwinding the substrate is performed by providing a suitable rotating means on the winding core 210A of the first roll 210 and rotating the first roll 210 by the rotating means. Alternatively, a suitable auxiliary roll 300 may be provided in the direction in which the substrate is transported from the first roll 210, and the substrate may be unwound by the rotating means of the auxiliary roll 300. Furthermore, by providing a rotating means on both the first winding core 210A and the auxiliary roll 300, the transparent substrate may be unwound while applying an appropriate tension to the substrate.
[0108] When the substrate unwound from the first roll 210 passes through the coating device 211A, the composition for forming a photo-alignment film is coated on the surface of the substrate by the coating device 211A. As the coating device 211A for continuously coating the composition for forming a photo-alignment film in this manner, gravure coating, die coating and flexography are preferable.
[0109] The substrate that has passed through the coating device 211A is transported to the drying oven 212A, where it is dried, and a first coating film is continuously formed on the substrate surface. For example, a hot air drying oven that combines a ventilation drying method and a heat drying method is used as the drying oven 212A. The set temperature of the drying oven 212A is determined according to the type of solvent contained in the composition for forming a photo-alignment film. The drying oven 212A may be composed of multiple zones with different set temperatures, or may be a drying oven in which multiple drying ovens with different set temperatures are installed in series.
[0110] The obtained first coating film is irradiated with polarized light by polarized UV irradiation device 213A, thereby obtaining a photo-alignment film.
[0111] Next, the substrate on which the photo-alignment film is formed passes through the coating device 211B. After the composition containing the dichroic dye, the polymerizable liquid crystal compound, and the solvent is applied onto the photo-alignment film by the coating device 211B, the composition passes through the drying oven 212B to obtain a second coating film in which the polymerizable liquid crystal compound is aligned. The drying oven 212B has a role of removing the solvent from the composition containing the polymerizable liquid crystal compound and the solvent applied onto the photo-alignment film, and also a role of providing heat energy so that the polymerizable liquid crystal compound contained in the composition is aligned. The drying oven 212B may be composed of multiple zones with different set temperatures, as with the drying oven 212A, or may be a drying oven in which multiple drying ovens with different set temperatures are installed in series.
[0112] The second coating film is transported to the active energy ray irradiation device 213B in a state where the polymerizable liquid crystal compound contained in the second coating film is aligned. The second coating film is irradiated with active energy rays in the active energy ray irradiation device 213B. The polymerizable liquid crystal compound is polymerized in the aligned state by the irradiation of active energy rays by the active energy ray irradiation device 213B.
[0113] The optical film thus continuously produced is wound around the second winding core 220A to obtain the form of the second roll 220. When winding, co-winding using an appropriate spacer may be performed.
[0114] In this manner, the substrate passes from the first roll 210 through the coating device 211A, the drying furnace 212A, the polarized UV irradiation device 213A, the coating device 211B, the drying furnace 212B, and the active energy ray irradiation device 213B in that order, whereby the optical film can be continuously produced in a roll-to-roll format. When no alignment film is included between the substrate and the light absorptive anisotropic film, the optical film can be produced by a similar production method that does not include the coating device 211A and the polarized UV irradiation device 213A.
[0115] <Three-dimensional optically absorptive anisotropic film> A three-dimensional optically absorptive anisotropic film can be formed by laminating the optically absorptive anisotropic film and a horizontal polarizing film. When laminating an optical film and a horizontal polarizing film, the optical film only needs to be laminated to the horizontal polarizing film on the optically absorptive anisotropic film side, and the substrate may be peeled off. A three-dimensional optically absorptive anisotropic film satisfies the following formula (6), when the absorption axis of the horizontal polarizing film is the x' axis, the transmission axis of the horizontal polarizing film is the y' axis, and the axis perpendicular to the x' and y' axes is the z' axis. In formula (6), Ax', Ay', and Az' each represent the absorbance at the maximum absorption wavelength of the dichroic dye in the light absorption anisotropic film. Ax' represents the absorbance of linearly polarized light vibrating in the x' direction, Ay' represents the absorbance of linearly polarized light vibrating in the y' direction, and Az' represents the absorbance of linearly polarized light vibrating in the z' direction. Ax' and Ay' are measured in the same manner as Ax and Ay. Az' can be calculated by the following formula (7): In the formula, Ay' (z=60) is the linearly polarized light oscillating in the y'-axis direction when the film is rotated 60° around the x'-axis as the rotation axis. represents the absorbance of Ax'>Az'>Ay' (6) Ay' (z=60)=Ay' cos60°+Az' sin60° (7)
[0116] <Horizontal polarizing film> The horizontal polarizing film has a polarizing function with an absorption axis parallel to the film surface. Examples of the horizontal polarizing film include a stretched film adsorbed with a dye having anisotropic absorption, and a film coated with a dye having anisotropic absorption. Examples of the dye having anisotropic absorption include a dichroic dye.
[0117] A stretched film having a dye having absorption anisotropy adsorbed thereon is usually produced through a process of uniaxially stretching a polyvinyl alcohol-based resin film, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, a process of treating the polyvinyl alcohol-based resin film having the dichroic dye adsorbed thereon with an aqueous boric acid solution, and a process of washing with water after the treatment with the aqueous boric acid solution.
[0118] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.
[0119] The degree of saponification of the polyvinyl alcohol resin is usually 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal or polyvinyl acetal modified with aldehydes can also be used. The degree of polymerization of the polyvinyl alcohol resin is usually 1,000 to 10,000, preferably 1,500 to 5,000.
[0120] The polyvinyl alcohol resin is formed into a film to obtain a raw film. The polyvinyl alcohol resin can be formed into a film by a known method. The thickness of the polyvinyl alcohol raw film is preferably 10 to 150 μm.
[0121] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. It is also possible to perform the uniaxial stretching in these multiple stages. In the uniaxial stretching, the film may be uniaxially stretched between rolls having different peripheral speeds, or may be uniaxially stretched using a heated roll. The uniaxial stretching may be dry stretching in which stretching is performed in the atmosphere, or wet stretching in which stretching is performed in a state in which the polyvinyl alcohol-based resin film is swollen using a solvent. The stretching ratio is usually 3 to 8 times.
[0122] Dyeing of a polyvinyl alcohol-based resin film with a dichroic dye is carried out by immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye. Examples of the dichroic pigment include iodine and dichroic organic dyes, with iodine being preferred. Examples of the dichroic organic dye include dichroic direct dyes made of disazo compounds such as CI DIRECT RED 39, and dichroic direct dyes made of compounds such as trisazo and tetrakisazo. The polyvinyl alcohol resin film is preferably immersed in water before the dyeing process.
[0123] When the dichroic dye is iodine, a method of dyeing a polyvinyl alcohol-based resin film by immersing it in an aqueous solution containing iodine and potassium iodide is usually adopted. The content of iodine in the aqueous solution is usually 0.01 to 1 part by mass per 100 parts by mass of water. The content of potassium iodide is usually 0.5 to 20 parts by mass per 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is usually 20 to 40°C. The immersion time in this aqueous solution (dyeing time) is usually 20 to 1,800 seconds.
[0124] When the dichroic pigment is a dichroic organic dye, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing a water-soluble dichroic dye is usually used. The content of the dichroic organic dye in the aqueous solution is usually 1×10 -4 ~10 parts by mass, preferably 1 × 10 -3 ~1 part by mass, more preferably 1 × 10 -3 ~1×10 -2 The amount is parts by mass. This aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing assistant. The temperature of the aqueous solution is usually 20 to 80° C. The immersion time in this aqueous solution (dyeing time) is usually 10 to 1,800 seconds.
[0125] The boric acid treatment after dyeing with a dichroic dye can usually be carried out by immersing the dyed polyvinyl alcohol-based resin film in an aqueous boric acid solution. The content of boric acid in the aqueous boric acid solution is usually 2 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. When iodine is used as the dichroic dye, the aqueous boric acid solution preferably contains potassium iodide, and the content of potassium iodide is usually 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. The immersion time in the aqueous boric acid solution is usually 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually 50°C or higher, preferably 50 to 85°C, and more preferably 60 to 80°C.
[0126] The polyvinyl alcohol-based resin film after the boric acid treatment is usually washed with water. The washing can be performed by immersing the boric acid-treated polyvinyl alcohol-based resin film in water. The temperature of the water used in the washing is usually 5 to 40°C. The immersion time is usually 1 to 120 seconds.
[0127] After washing with water, the film is dried to obtain a horizontal polarizing film. The drying can be performed using a hot air dryer or a far infrared heater. The temperature of the drying is usually 30 to 100°C, preferably 50 to 80°C. The time of the drying is usually 60 to 600 seconds, preferably 120 to 600 seconds. The moisture content of the horizontal polarizing film is reduced to a practical level by the drying. The moisture content is usually 5 to 20% by weight, preferably 8 to 15% by weight. If the moisture content is less than 5% by weight, the flexibility of the horizontal polarizing film is lost, and the horizontal polarizing film may be damaged or broken after drying. If the moisture content exceeds 20% by weight, the thermal stability of the horizontal polarizing film may be deteriorated.
[0128] The polyvinyl alcohol resin film is then uniaxially stretched, dyed with a dichroic dye, treated with boric acid, washed with water and dried to obtain a horizontal polarizing film having a thickness preferably of 5 to 40 μm.
[0129] Examples of the film coated with a dye having anisotropic absorption include a film obtained by coating a composition containing a dichroic dye having liquid crystal properties, or a composition containing a dichroic dye and a polymerizable liquid crystal. It is preferable to use the same dichroic dye as that contained in the light absorption anisotropic film.
[0130] The film coated with the dye having absorption anisotropy is preferably thin, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the film is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 to 3 μm.
[0131] Specific examples of films coated with a dye having absorption anisotropy include the films described in JP-A-2012-33249 and the like.
[0132] A polarizing plate is obtained by laminating a transparent protective film on at least one surface of the horizontal polarizing film via an adhesive. The transparent protective film is preferably the same transparent film as the above-mentioned substrate.
[0133] As the configuration of the three-dimensional optically absorptive anisotropic film, in addition to the present optically absorptive anisotropic film and horizontal polarizing film, any appropriate layer used in the configuration of a liquid crystal display device, such as an antiglare layer, an antireflection layer, an antistatic layer, a light diffusion control layer, a brightness enhancing layer, a reflective layer, and a semi-transmissive layer, can be used. EXAMPLES
[0134] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0135] Example 1 [Preparation of Optically Absorbent Anisotropic Composition] The following components were mixed and stirred at 80°C for 1 hour to obtain an optically absorptive anisotropic composition. The dichroic dye used was an azo dye described in the examples of JP2013-101328A. The polymerizable liquid crystal compounds represented by formulae (1-6) and (1-7) were synthesized according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). Polymerizable liquid crystal compound: TIFF0007557518000015.tif17150 75 copies TIFF0007557518000016.tif17138 25 copies Dichroic dye 1: TIFF0007557518000017.tif1188 2.8 parts Polymerization initiator; 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals) 6 parts Leveling agent; Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 0.3 parts Solvent: o-xylene 250 parts
[0136] [Measurement of phase transition temperature of polymerizable liquid crystal compounds] The phase transition temperature was confirmed by observing the texture with a polarizing microscope (BX-51, manufactured by Olympus Corporation) while heating the compound on a glass substrate on which an alignment film was formed. The polymerizable liquid crystal compound represented by formula (1-6) exhibited a smectic A phase from a crystalline phase at 95°C, a nematic phase at 111°C, and an isotropic liquid phase at 113°C during heating. It was confirmed that the compound exhibited a nematic phase at 112°C, a smectic A phase at 110°C, and a smectic B phase at 94°C during cooling. The polymerizable liquid crystal compound represented by formula (1-7) exhibited a smectic A phase from a crystalline phase at 81°C, a nematic phase at 121°C, and an isotropic liquid phase at 137°C during heating. During cooling, it was confirmed that the liquid crystal showed a phase transition to a nematic phase at 133°C, a phase transition to a smectic A phase at 118°C, and a phase transition to a smectic B phase at 78°C. In the same manner, the texture of the thermotropic nematic liquid crystal LC242 manufactured by BASF was observed. The LC242 exhibited a nematic phase, but did not exhibit a smectic phase.
[0137] [Production of optically absorptive anisotropic films] The optically absorptive anisotropic composition was applied onto a 50 mm x 50 mm glass plate using a spin coater, and then dried for 1 minute in a drying oven set at 110°C to obtain a dried coating film in which the polymerizable liquid crystal compound and the dichroic dye were oriented. This dried coating film was naturally cooled to room temperature, and then irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm) using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.). 2 ) to polymerize the polymerizable liquid crystal compound, thereby obtaining an optically absorptive anisotropic film 1.
[0138] [Evaluation of optically absorbing anisotropic films] [Three-dimensional absorbance measurement] The absorbance of the optically absorptive anisotropic film 1 was measured as follows. Using an apparatus in which a folder with a prism polarizer was set in a spectrophotometer (UV-3150 manufactured by Shimadzu Corporation), the three-dimensional absorbance at the wavelength showing the maximum absorption was measured in the wavelength range of 380 to 680 nm at 2 nm steps by the double-beam method. Here, the three-dimensional absorbance means the absorbances (Ax, Ay, Az) in each direction with respect to linearly polarized light when an arbitrary direction in the film plane is the x-axis, the direction orthogonal to the x-axis in the film plane is the y-axis, and the film thickness direction of the film is the z-axis. Specifically, the measurement was performed by rotating the sample with respect to the linearly polarized light that is the measurement light. Also, since the absorbance in the z direction is difficult to measure because, by definition, light is incident from the side surface of the sample, the absorbance in the Az direction was estimated by tilting the x-y plane of the sample by 30° and 60° with respect to the vibration plane of the linearly polarized light that is the measurement light. Specifically, Ax(z = 30) and Ax(z = 60) were measured by making the same linearly polarized light incident as when Ax was measured with the sample rotated by 30° and 60° so as to include the y-axis, and similarly, Ay(z = 30) and Ay(z = 60) were measured by making the same linearly polarized light incident as when Ay was measured with the sample rotated by 30° and 60° so as to include the x-axis. Note that when there is no absorption anisotropy in the x-y plane, that is, when Ax and Ay are equal, Ax(z = 30) = Ay(z = 30) and Ax(z = 60) = Ay(z = 60), so Ax(z = 30) and Ay(z = 30) were designated as A(z = 30), and Ax(z = 60) and Ay(z = 60) were designated as A(z = 60). That is, when in the relationship of A(z = 30) < A(z = 60), the relationship of A(z = 30) < A(z = 60) < A(z = 90) = Az is satisfied. Further, if A(z = 30) > (Ax + Ay) / 2 or A(z = 60) > (Ax + Ay) / 2, then inevitably the following formula (1) is satisfied. Az > (Ax + Ay) / 2 (1) As a result of measuring the sample of Example 1 of this case, the three-dimensional absorbances at the wavelength 526 nm, which is the wavelength of maximum absorption, were Ax = 0.029, Ay = 0.029, A(z = 30) = 0.146, and A(z = 60) = 0.502. That is, the optically absorptive anisotropic film 1 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 17.3 > 5 (2) Ay(z=60) / Ay = 17.3 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 1 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.7 μm.
[0139] Example 2 An optically absorptive anisotropic film 2 was prepared in the same manner as in Example 1, except that dichroic dye 2 was used instead of dichroic dye 1. Dichroic dye 2: TIFF0007557518000018.tif14150 2.8 parts
[0140] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 2 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 606 nm was Ax = 0.023, Ay = 0.023, A(z = 30) = 0.134, and A(z = 60) = 0.417. That is, the optically absorptive anisotropic film 2 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 18.1 > 5 (2) Ay(z=60) / Ay = 18.1 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 2 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.6 μm.
[0141] Example 3 An optically absorptive anisotropic film 3 was prepared in the same manner as in Example 1, except that dichroic dye 3 was used instead of dichroic dye 1. Dichroic dye 3: TIFF0007557518000019.tif13150 2.8 parts
[0142] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 3 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 620 nm was Ax = 0.050, Ay = 0.050, A(z = 30) = 0.226, and A(z = 60) = 0.647. That is, the optically absorptive anisotropic film 3 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 12.9 > 5 (2) Ay(z=60) / Ay = 12.9 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 3 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.8 μm.
[0143] Example 4 An optically absorptive anisotropic film 4 was prepared in the same manner as in Example 1, except that dichroic dye 4 was used instead of dichroic dye 1. Dichroic dye 4: TIFF0007557518000020.tif12101 2.8 parts
[0144] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 4 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 402 nm was Ax = 0.086, Ay = 0.086, A(z = 30) = 0.193, and A(z = 60) = 0.525. That is, the optically absorptive anisotropic film 4 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 6.1 > 5 (2) Ay(z=60) / Ay = 6.1 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 4 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.7 μm.
[0145] Example 5 An optically absorptive anisotropic film 5 was prepared in the same manner as in Example 1, except that dichroic dye 5 was used instead of dichroic dye 1. Dichroic dye 5: TIFF0007557518000021.tif13100 2.8 parts
[0146] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 5 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 546 nm was Ax = 0.020, Ay = 0.020, A(z = 30) = 0.105, and A(z = 60) = 0.333. That is, the optically absorptive anisotropic film 5 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 16.7 > 5 (2) Ay(z=60) / Ay = 16.7 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 5 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.7 μm.
[0147] Example 6 [Production of composition for forming alignment film] Propylene glycol monomethyl ether was added to the alignment polymer to obtain a composition for forming an alignment film. The solid content of the alignment polymer is calculated by converting the solid content from the concentration described in the delivery specification. Oriented polymer: SunEver (registered trademark) SE-610 (manufactured by Nissan Chemical Industries, Ltd.) 0.3 parts (1.0%) Propylene glycol monomethyl ether: 27.7 parts
[0148] [Production of optically absorptive anisotropic films] A polyethylene terephthalate film (Mitsubishi Plastics, Diafoil T140E25) was cut to 80 x 80 mm, and its surface was subjected to a corona treatment (AGF-B10, Kasuga Electric Co., Ltd.). The corona-treated film surface was coated with a composition for forming an alignment film using a bar coater, and then dried for 1 minute in a drying oven set at 120°C to obtain an alignment film. The same liquid crystal cured film forming composition as used in Example 1 was coated on the obtained alignment film using a bar coater, and then dried for 1 minute in a drying oven set at 110°C, and then irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm) using a high-pressure mercury lamp (Uniquer VB-15201BY-A, Ushio Electric Co., Ltd.). 2 ) to polymerize the polymerizable liquid crystal compound, thereby obtaining an optically absorptive anisotropic film 6.
[0149] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 5 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 526 nm was Ax = 0.040, Ay = 0.040, A(z = 30) = 0.184, and A(z = 60) = 0.602. That is, the optically absorptive anisotropic film 6 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 15.1 > 5 (2) Ay(z=60) / Ay = 15.1 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 6 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.2 μm.
[0150] Example 7 An optically absorptive anisotropic film 7 was prepared in the same manner as in Example 6, except that dichroic dye 2 was used instead of dichroic dye 1.
[0151] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 7 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 608 nm was Ax = 0.032, Ay = 0.032, A(z = 30) = 0.184, and A(z = 60) = 0.588. That is, the optically absorptive anisotropic film 7 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 18.4 > 5 (2) Ay(z=60) / Ay = 18.4 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 7 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.2 μm.
[0152] Example 8 An optically absorptive anisotropic film 8 was prepared in the same manner as in Example 6, except that dichroic dye 3 was used instead of dichroic dye 1.
[0153] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 8 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 622 nm was Ax = 0.078, Ay = 0.078, A(z = 30) = 0.291, and A(z = 60) = 0.860. That is, the optically absorptive anisotropic film 8 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 11.0 > 5 (2) Ay(z=60) / Ay = 11.0 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 8 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.3 μm.
[0154] Comparative Example 1 An optically absorptive anisotropic film 9 was prepared in the same manner as in Example 2, except that thermotropic nematic liquid crystal LC242 manufactured by BASF was used instead of the polymerizable liquid crystal compounds (1-6) and (1-7). This sample did not provide transparency, and molecular orientation of the polymerizable liquid crystal and dichroic dye was not obtained. TIFF0007557518000022.tif20133
[0155] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 9 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 560 nm was Ax = 0.327, Ay = 0.327, A(z = 30) = 0.317, and A(z = 60) = 0.312. That is, the optically absorptive anisotropic film 9 does not satisfy the formulas (1), (2), and (3) as follows. Az< A(z=60)< A(z=30)< (Ax+Ay) / 2 Ax(z=60) / Ax = 1.0 Ay(z=60) / Ay = 1.0 [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 9 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 1.7 μm.
[0156] Comparative Example 2 An optically absorptive anisotropic film 10 was prepared in the same manner as in Example 6, except that a thermotropic nematic liquid crystal LC242 (manufactured by BASF) was used instead of the polymerizable liquid crystal compounds (1-6) and (1-7). TIFF0007557518000023.tif20133
[0157] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 10 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 488 nm was Ax = 0.072, Ay = 0.072, A(z = 30) = 0.133, and A(z = 60) = 0.275. That is, the optically absorptive anisotropic film 10 satisfies the formula (1) as follows, but does not satisfy the formulas (2) and (3). Az>A(z=60)> A(z=30)>(Ax+Ay) / 2 Ax(z=60) / Ax = 3.8 Ay(z=60) / Ay = 3.8 [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 10 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.1 μm.
[0158] Comparative Example 3 An optically absorptive anisotropic film 11 was prepared in the same manner as in Example 7, except that a thermotropic nematic liquid crystal LC242 (manufactured by BASF) was used instead of the polymerizable liquid crystal compounds (1-6) and (1-7). TIFF0007557518000024.tif20133
[0159] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 11 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 560 nm was Ax = 0.071, Ay = 0.071, A(z = 30) = 0.125, and A(z = 60) = 0.275. That is, the optically absorptive anisotropic film 10 satisfies the formula (1) as follows, but does not satisfy the formulas (2) and (3). Az>A(z=60)> A(z=30)>(Ax+Ay) / 2 Ax(z=60) / Ax = 3.9 Ay(z=60) / Ay = 3.9 [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 11 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.1 μm.
[0160] Comparative Example 4 An optically absorptive anisotropic film 12 was prepared in the same manner as in Example 8, except that a thermotropic nematic liquid crystal LC242 (manufactured by BASF) was used instead of the polymerizable liquid crystal compounds (1-6) and (1-7). TIFF0007557518000025.tif20133
[0161] [Three-dimensional absorbance measurement] As in Example 1, the three-dimensional absorbance of the optically absorptive anisotropic film 12 was measured. As a result, the three-dimensional absorbance at the maximum absorption wavelength of 594 nm was Ax = 0.133, Ay = 0.133, A(z = 30) = 0.220, and A(z = 60) = 0.460. That is, the optically absorptive anisotropic film 12 satisfies the formula (1) as follows, but does not satisfy (2) and (3). Az>A(z=60)> A(z=30)>(Ax+Ay) / 2 Ax(z=60) / Ax = 3.5 Ay(z=60) / Ay = 3.5 [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 12 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.1 μm.
[0162] Example 9 An optically absorptive anisotropic film 13 was prepared in the same manner as in Example 6, except that dichroic dye 1, dichroic dye 3, and dichroic dye 4 were used simultaneously in place of dichroic dye 1.
[0163] [Three-dimensional absorbance measurement] As a result of measuring the three-dimensional absorbance of the optically absorptive anisotropic film 13 in the same manner as in Example 1, maximum absorptions due to the three types of dyes were obtained. First absorption: The three-dimensional absorbance at a wavelength of 400 nm was Ax = 0.115, Ay = 0.115, A(z = 30) = 0.274, and A(z = 60) = 0.692. That is, the optically absorptive anisotropic film 13 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 6.0 > 5 (2) Ay(z=60) / Ay = 6.0 > 5 (3) Second Absorption: The three-dimensional absorbance at a wavelength of 526 nm was Ax = 0.062, Ay = 0.062, A(z = 30) = 0.220, and A(z = 60) = 0.639. That is, the optically absorptive anisotropic film 13 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 10.2 > 5 (2) Ay(z=60) / Ay = 10.2 > 5 (3) Third Absorption: The three-dimensional absorbance at a wavelength of 622 nm was Ax = 0.049, Ay = 0.049, A(z = 30) = 0.187, and A(z = 60) = 0.468. That is, the optically absorptive anisotropic film 13 satisfies the following formulas (1), (2), and (3). Az> A(z=60)> A(z=30)> (Ax+Ay) / 2 (1) Ax(z=60) / Ax = 11.3 > 5 (2) Ay(z=60) / Ay = 11.3 > 5 (3) [Film thickness measurement] The thickness of the liquid crystal cured film in the optically absorptive anisotropic film 13 was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2.3 μm.
[0164] Example 10 [Manufacturing of polarizing plates] A polyvinyl alcohol film having an average degree of polymerization of about 2,400, a degree of saponification of 99.9 mol% or more, and a thickness of 75 μm was immersed in pure water at 30°C, and then immersed in an aqueous solution having a weight ratio of iodine / potassium iodide / water of 0.02 / 2 / 100 at 30°C to perform iodine dyeing (iodine dyeing step). The polyvinyl alcohol film that had undergone the iodine dyeing step was immersed in an aqueous solution having a weight ratio of potassium iodide / boric acid / water of 12 / 5 / 100 at 56.5°C to perform boric acid treatment (boric acid treatment step). The polyvinyl alcohol film that had undergone the boric acid treatment step was washed with pure water at 8°C, and then dried at 65°C to obtain a horizontal polarizing film (thickness 27 μm after stretching) in which iodine was adsorbed and aligned in the polyvinyl alcohol. At this time, stretching was performed in the iodine dyeing step and the boric acid treatment step. The total stretching ratio in this stretching was 5.3 times. The obtained horizontal polarizing film and a saponified triacetyl cellulose film (KC4UYTAC 40 μm, manufactured by Konica Minolta) were bonded together by nip rolls via a water-based adhesive. The resulting laminate was dried at 60° C. for 2 minutes while maintaining a tension of 430 N / m to obtain a polarizing plate (1) having a triacetyl cellulose film as a protective film on one side. The water-based adhesive was prepared by adding 3 parts of carboxyl group-modified polyvinyl alcohol (Kuraray Poval KL318, manufactured by Kuraray) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650, manufactured by Sumika Chemtex, aqueous solution with a solid content of 30%) to 100 parts of water. The polarizing plate and the liquid crystal cured film side of the optically absorptive anisotropic film 13 obtained in Example 9 were bonded together via a pressure-sensitive adhesive to produce a three-dimensional optically absorptive anisotropic film as shown in FIG. 3.
[0165] [Three-dimensional absorbance measurement] The three-dimensional absorbance of the obtained composite polarizing plate was measured in the same manner as in Example 1. The three-dimensional absorbance here refers to the absorbance in each direction (Ax', Ay', Az') when the absorption axis of the polarizing plate is the direction of x', the transmission axis direction of the polarizing plate is the direction of y', and the film thickness direction of the liquid crystal cured film is the direction of z'. The magnitude relationship between Ax', Ay', and Az' was determined by measuring Ax' and Ax' (z=60), as well as Ay' and Ay' (z=60). Second Absorption: The three-dimensional absorbance at a wavelength of 526 nm was Ax'=3.158, Ay'=0.065, and Ay'(z=60)=0.614. Since the relationship is Ay' (z=60)=Ay' cos60°+Az' sin60°, Az' is calculated to be 0.671. Therefore, it was confirmed that formula (6) is satisfied. Ax'> Az'> Ay' (6)
[0166] As shown in Figure 4, a polarizing plate was attached to the rear side of the LCD panel via a pressure-sensitive adhesive, and then a three-dimensional optically absorptive anisotropic film was attached to the front side of the LCD panel via a pressure-sensitive adhesive so that the polarizing plate side faced the panel. The appearance was evaluated, and it was confirmed that while clear visibility was maintained from the front, visibility from the side was reduced, providing an anti-peeping function. [Industrial Applicability]
[0167] The optically absorptive anisotropic film of the present invention is thin and can be produced by a simple manufacturing method, and is useful as a material for imparting a more effective anti-peek function to displays of mobile phones, bank ATMs, and the like. [Explanation of symbols]
[0168] 210 Roll 1 210A core 220 Roll 2 220A core 211A, 211B Coating equipment 212A,212B Drying oven 213A Polarized UV irradiation device 213B Active energy ray irradiation equipment 300 Auxiliary Roll 1. Optically Absorbing Anisotropic Film 2 Adhesive layer 3 Horizontal polarizing film 4. Three-dimensional optically absorbing anisotropic film 5 LCD panel
Claims
1. A three-dimensional optically absorptive anisotropic film is formed by laminating an optically absorptive anisotropic film, which is a cured film of a composition containing a dichroic dye and a liquid crystal compound, and a horizontal polarizing film, the liquid crystalline compound forms a smectic liquid crystal phase, When the optically absorptive anisotropic film has an x-axis in any direction within the film plane, a y-axis in a direction perpendicular to the x-axis within the film plane, and a z-axis in a film thickness direction perpendicular to the x-axis and y-axis, the optical absorbance of the film satisfies the following formulas (1), (2), and (3): the horizontal polarizing film is a cured film of a composition containing a dichroic dye and a liquid crystalline compound, or a cured film of a composition containing a dichroic dye having liquid crystal properties, The three-dimensional optically absorptive anisotropic film satisfies the following formula (6) when the absorption axis of the horizontal polarizing film is defined as the x' axis, the transmission axis of the horizontal polarizing film is defined as the y' axis, and the axis perpendicular to the x' axis and the y' axis is defined as the z' axis: Az>(Ax+Ay) / 2 (1) Ax (z=60) / Ax≧11.0 (2) Ay (z=60) / Ay≧11.0 (3) Ax'>Az'>Ay' (6) (Ax, Ay, Az, Ax(z=60) and Ay(z=60) are all absorbances at the absorption maximum wavelengths of the dichroic dyes in the optically absorptive anisotropic film, Ax represents the absorbance of linearly polarized light vibrating in the x-axis direction, Ay represents the absorbance of linearly polarized light vibrating in the y-axis direction, Az represents the absorbance of linearly polarized light vibrating in the z-axis direction, Ax (z=60) represents the absorbance of linearly polarized light oscillating in the x-axis direction when the film is rotated 60° around the y-axis as the rotation axis, Ay (z=60) represents the absorbance of linearly polarized light oscillating in the y-axis direction when the film is rotated 60° around the x-axis as the rotation axis, Ax', Ay', and Az' are all absorbances of the three-dimensional optically absorptive anisotropic film at the absorption maximum wavelength of the dichroic dye in the optically absorptive anisotropic film, Ax' represents the absorbance of linearly polarized light vibrating in the x' direction, Ay′ represents the absorbance of linearly polarized light vibrating in the y′ direction, Az' represents the absorbance of linearly polarized light vibrating in the z' direction.)
2. 2. The three-dimensional optically absorptive anisotropic film according to claim 1, wherein the liquid crystalline compound forms a high-order smectic liquid crystal phase.
3. 3. The three-dimensional optically absorptive anisotropic film according to claim 1, which exhibits a Bragg peak in X-ray diffraction measurement.
4. 4. The three-dimensional optically absorptive anisotropic film according to claim 1, wherein the dichroic dye in the optically absorptive anisotropic film has a maximum absorption wavelength in the range of 500 nm to 600 nm.
5. 5. The three-dimensional optically absorptive anisotropic film according to claim 1, wherein the optically absorptive anisotropic film contains at least three kinds of dichroic dyes having different maximum absorption wavelengths.
6. 6. The three-dimensional optically absorptive anisotropic film according to claim 1, wherein the film thickness of the optically absorptive anisotropic film is 5 μm or less.
7. 7. The three-dimensional optically absorptive anisotropic film according to claim 1, wherein the optically absorptive anisotropic film is laminated on the horizontal polarizing film via a pressure sensitive adhesive or a bonding agent.
Citation Information
Patent Citations
Visible angle control member and its manufacturing method
JP2005215435A
Viewing angle control system and image display device
JP2009145776A
Polarizing plate, and liquid crystal display using the same
JP2010033050A