Aluminum wire with aluminum crimp terminal

The aluminum electric wire with a crimp terminal addresses thermal expansion issues by structuring the crimp part with distinct grain sizes and hardness ratios, ensuring reliable connections with reduced force and improved durability.

JP7558798B2Active Publication Date: 2024-10-01FURUKAWA ELECTRIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020214574
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-10-01
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing methods for connecting aluminum conductor wires to terminals require significant force and result in poor workability due to thermal expansion issues, leading to potential misalignment and increased electrical resistance.

Method used

The aluminum electric wire with an aluminum crimp terminal features a conductor crimp part where the conductor is crimped perpendicular to the wire, with an inner region having an average crystal grain size of less than 50 μm and an outer region of 50 μm or more, along with specific hardness ratios to maintain connection reliability with reduced crimping force.

Benefits of technology

This design ensures stable connection reliability and suppresses temperature rise and electrical resistance increases, improving workability and durability even with lighter crimping tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558798000004
    Figure 0007558798000004
  • Figure 0007558798000005
    Figure 0007558798000005
  • Figure 0007558798000006
    Figure 0007558798000006
Patent Text Reader

Abstract

To provide an aluminum wire with an aluminum crimp terminal which has good connection reliability between an aluminum wire and an aluminum crimp terminal even when the force of crimping the aluminum crimp terminal is reduced.SOLUTION: In an aluminum wire with an aluminum crimp terminal having a conductor crimping portion in which a conductor of an aluminum wire is crimped to a tubular insertion portion of the aluminum crimping terminal, in the cross section of the conductor crimping portion perpendicular to the longitudinal direction of the aluminum wire, the insertion portion of the aluminum crimp terminal includes an inner region which is in contact with the conductor of the aluminum wire and has an average crystal grain size of less than 50 μm, and an outer region adjacent to the outside of the inner region and having an average crystal grain size of 50 μm or more in a crimping recess facing part facing a crimping recess.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum electric wire with an aluminum crimp terminal. [Background technology]

[0002] Generally, copper-based materials such as copper and copper alloys, which have high electrical conductivity, are used for the conductors of electric power distribution cables. In recent years, aluminum conductors (hereinafter also referred to as aluminum conductors) are sometimes used from the viewpoint of weight reduction.

[0003] On the other hand, when connecting an aluminum conductor and a copper terminal, which are dissimilar metals, a difference in thermal expansion between the conductor and the terminal occurs due to a rise in temperature when electricity is passed through the conductor, which can cause a mechanical misalignment at the connection. If a misalignment occurs at the connection, the oxide coating of the aluminum conductor, which had a natural oxide coating in the air before the misalignment, may come into contact with the copper terminal, or the connection part of the aluminum conductor that was in contact with the copper terminal before the misalignment may separate from the copper terminal and become non-contact, oxidizing in the air, which may increase the electrical resistance of the connection, leading to further heat generation or, in the worst case, a fire.

[0004] To avoid such problems, aluminum terminals are used instead of copper terminals for connecting to aluminum conductors. For example, an aluminum terminal is mainly composed of a tubular insertion part into which the conductor of the aluminum electric wire is inserted and connected, and a flat shuttlecock part having a bolt hole for connecting to a terminal block.

[0005] For example, Patent Document 1 describes an electric wire with a terminal, which includes an electric wire including a conductor and an insulating layer, with the conductor exposed at an end, and a terminal having a crimping portion that crimps and connects to the exposed conductor, the terminal being made of an aluminum material and the crimping portion having a tensile strength of 80 MPa or less. Patent Document 2 describes an electric wire with a terminal, which includes an electric wire including a conductor made of an elemental wire and a coating, and a compression terminal attached to the end of the conductor, the elemental wire being made of a first material mainly composed of aluminum, at least a portion of the compression terminal that contacts the conductor being made of a second material mainly composed of aluminum, and the first material having a tensile strength greater than that of the second material.

[0006] As described above, in Patent Documents 1 and 2, an aluminum conductor is inserted into an insertion portion, and pressure is applied from the outside to multiple points of the insertion portion to crimp the insertion portion, thereby connecting the electric wire and the crimp terminal. However, in these methods, pressure is applied to multiple points of the insertion portion to compress and connect the insertion portion of the terminal and the electric wire, so a large force is required to connect the terminal and the electric wire. Furthermore, the device for compressing the terminal is large-scale, and the workability is poor when implementing these methods at an electric wire installation site where wiring space is limited. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-169364 A [Patent Document 2] JP 2020-27758 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present disclosure is to provide an aluminum electric wire with an aluminum crimp terminal that has good connection reliability between the aluminum electric wire and the aluminum crimp terminal even when the force used to crimp the aluminum crimp terminal is reduced. [Means for solving the problem]

[0009] [1] An aluminum electric wire with an aluminum crimp terminal having a conductor crimping portion in which a conductor of an aluminum electric wire is crimped into a tubular insertion portion of an aluminum crimp terminal, characterized in that in a cross section of the conductor crimping portion perpendicular to the longitudinal direction of the aluminum electric wire, the insertion portion of the aluminum crimp terminal has, at a crimp recess facing portion facing the crimp recess, an inner region in contact with the conductor of the aluminum electric wire and having an average crystal grain size of less than 50 μm, and an outer region adjacent to the outside of the inner region and having an average crystal grain size of 50 μm or more. [2] The aluminum electric wire with aluminum crimp terminal described in [1] above, wherein, in the cross section, a ratio (h1 / (h1+h2))×100 of the thickness h1 of the inner region to the total thickness (h1+h2) of the thickness h1 of the inner region and the thickness h2 of the outer region is 70% or less. [3] The aluminum electric wire with aluminum crimp terminal according to [1] or [2] above, wherein the average Vickers hardness of the inner region in the cross section is 25 or more. [4] The aluminum electric wire with aluminum crimp terminal according to any one of the above [1] to [3], wherein the average Vickers hardness of the inner region in the cross section is 50 or less, and the average Vickers hardness of the outer region in the cross section is less than 25. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide an aluminum electric wire with an aluminum crimp terminal in which the connection reliability between the aluminum electric wire and the aluminum crimp terminal is good even if the force for crimping the aluminum crimp terminal is reduced. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a perspective view showing an example of a configuration of a main part of an aluminum electric wire with an aluminum crimp terminal according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line AA of FIG. [Diagram 3] FIG. 3 is an optical microscope photograph of a cross section of a conductor crimped portion constituting the aluminum electric wire with aluminum crimp terminal produced in Example 1. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, a detailed description will be given based on an embodiment.

[0013] As a result of extensive research, the inventors have discovered that by focusing on the inner structure of the insertion portion of the aluminum crimp terminal, it is possible to maintain good connection reliability between an aluminum electric wire and an aluminum crimp terminal even if the force used to crimp the aluminum crimp terminal is reduced, and have completed the present disclosure based on this finding.

[0014] An aluminum electric wire with an aluminum crimp terminal of an embodiment is an aluminum electric wire with an aluminum crimp terminal having a conductor crimping portion in which a conductor of an aluminum electric wire is crimped into a tubular insertion portion of an aluminum crimp terminal, and in a cross section of the conductor crimping portion perpendicular to the longitudinal direction of the aluminum electric wire, the insertion portion of the aluminum crimp terminal has, at a crimp recess facing portion facing the crimp recess, an inner region that contacts the conductor of the aluminum electric wire and has an average crystal grain size of less than 50 μm, and an outer region adjacent to the outside of the inner region and having an average crystal grain size of 50 μm or more.

[0015] Fig. 1 is a perspective view showing an example of a main configuration of an aluminum electric wire with an aluminum crimp terminal of an embodiment. Fig. 2 is a cross-sectional view taken along line AA of Fig. 1. As shown in Figs. 1 and 2, an aluminum electric wire 1 with an aluminum crimp terminal has a conductor crimping portion 2. In the conductor crimping portion 2, a conductor 12 of an aluminum electric wire 10 is crimped to a tubular insertion portion 21 of an aluminum crimp terminal 20.

[0016] 1, an aluminum electric wire 10 has a conductor wire 12, an insulating coating 13 covering the outer periphery of the conductor wire 12, and a sheath 14 covering the outer periphery of the insulating coating 13. At one end of the aluminum electric wire 10, the insulating coating 13 covering the outer periphery of the conductor wire 12 and the sheath 14 covering the outer periphery of the insulating coating 13 are stripped from the aluminum electric wire 10, exposing the conductor wire 12.

[0017] One end of the aluminum crimp terminal 20 is provided with a tubular insertion portion 21 into which the conductor 12 exposed at one end of the aluminum electric wire 10 is inserted. When the insertion portion 21 of the aluminum crimp terminal 20 is crimped with the conductor 12 of the aluminum electric wire 10 inserted into the insertion portion 21 of the aluminum crimp terminal 20, the insertion portion 21 is crimped to the aluminum electric wire 10 so as to cover the outer periphery of the conductor 12. When the insertion portion 21 of the aluminum crimp terminal 20 is crimped to the conductor 12, a conductor crimping portion 2 is formed. The aluminum crimp terminal 20 is electrically connected to the conductor 12 via the conductor crimping portion 2.

[0018] A flat shuttlecock portion 22 having, for example, a through hole 22a is provided on the other end side of the aluminum crimp terminal 20. By inserting a fastening member such as a bolt through the through hole 22a of the shuttlecock portion 22, the aluminum crimp terminal 20 is electrically connected to a terminal block (not shown).

[0019] Conductor wire 12 of aluminum electric wire 10 is composed of at least one or more element wires 11. Conductor wire 12 may be a stranded wire in which a plurality of element wires 11 are twisted together as shown in FIG.

[0020] The outer diameter of the cross section of the conductor 12 perpendicular to the longitudinal direction L of the aluminum electric wire 10 may be circular as shown in Fig. 1, or may be flat. The conductor 12 may be compressed.

[0021] With respect to the conductor 12, from the viewpoint of reducing electrical resistance and suppressing heat generation during energization, the composition of the wires 11 constituting the aluminum electric wire 10, i.e., the composition of the conductor 12, contains 99.5 mass % or more, preferably 99.7 mass % or more of Al (aluminum). For example, the conductor 12 is preferably A1050 or A1070.

[0022] Furthermore, the composition of the conductive wire 12 may contain, in addition to Al, one or more elements selected from the group consisting of Ti, B, V, Fe, Si, Cu, Mn, Mg, and Zn.

[0023] When the total content of one or more elements selected from the group consisting of Ti (titanium) and B (boron) is 0.001% by mass or more, the crystal grains in the aluminum ingot obtained in the casting process can be refined, and cracks and breaks can be suppressed during the subsequent cold drawing. When the total content of the above elements is 0.100% by mass or less, high ductility and high electrical conductivity can be maintained.

[0024] When the V (vanadium) content is 0.001% by mass or more, impurities can be easily removed from the molten metal during the casting process.When the V content is 0.100% by mass or less, the conductive wire 12 can maintain high ductility and high electrical conductivity.

[0025] When the total content of one or more elements selected from the group consisting of Fe (iron), Si (silicon), Cu (copper), Mn (manganese), Mg (magnesium) and Zn (zinc) is 0.001% by mass or more, the tensile strength and fatigue strength of the conductor wire 12 are increased. Therefore, even if the aluminum electric wire 10 is used in a bent state after connection, such as in a cab-tire cable or elevator cable, breakage of the conductor wire 12 due to bending can be suppressed. When the total content of the above elements is less than 0.500% by mass, deterioration of wire drawability and deterioration of electrical conductivity can be suppressed.

[0026] The remainder other than the above-mentioned components are unavoidable impurities. The unavoidable impurities may be unavoidably contained in the manufacturing process, and depending on the content, may be a factor in reducing the electrical conductivity and strength of the conductor 12. Therefore, it is preferable that the content of the unavoidable impurities is small. Examples of the unavoidable impurities include elements such as Li (lithium), Ni (nickel), and Cr (chromium). The upper limit of the content of the unavoidable impurities is preferably less than 0.500 mass% in terms of the total of the above elements.

[0027] In order to reduce electrical resistance and suppress heat generation during energization, the aluminum crimp terminal 20 contains 99.5% by mass or more, and preferably 99.7% by mass or more of Al in its composition. For example, the conductive wire 12 is preferably A1050 or A1070.

[0028] Furthermore, the composition of the aluminum crimp terminal 20 may contain, in addition to Al, one or more elements selected from the group consisting of Ti, B, V, Fe, Si, Cu, Mn, Mg, and Zn.

[0029] When the total content of one or more elements selected from the group consisting of Ti and B is 0.001% by mass or more, the crystal grains in the aluminum ingot obtained in the casting process can be refined, and cracks during the subsequent cold drawing can be suppressed.When the total content of the above elements is 0.100% by mass or less, high ductility and high electrical conductivity can be maintained.

[0030] When the V content is 0.001% by mass or more, impurities can be easily removed from the molten metal during the casting process.When the V content is 0.100% by mass or less, the aluminum crimp terminal 20 can maintain high ductility and high electrical conductivity.

[0031] When the total content of one or more elements selected from the group consisting of Fe, Si, Cu, Mn, Mg, and Zn is 0.001% by mass or more, the durability strength of the aluminum crimp terminal 20 is increased. Therefore, the aluminum crimp terminal 20, which is repeatedly connected and used and has been made smaller and thinner to reduce weight, can be prevented from breaking or bending. When the total content of the above elements is less than 0.500% by mass, the decrease in electrical conductivity can be prevented.

[0032] The remainder other than the above-mentioned components are unavoidable impurities. The content of unavoidable impurities may be a factor in reducing the electrical conductivity and strength of the aluminum crimp terminal 20, so it is preferable that the content of unavoidable impurities is small. Examples of unavoidable impurities include elements such as Li, Ni, and Cr. The upper limit of the content of the unavoidable impurities is preferably less than 0.500 mass% in terms of the total of the above elements.

[0033] 1 and 2, in a cross section of the conductor crimping portion 2 perpendicular to the longitudinal direction L of the aluminum electric wire 10, the insertion portion 21 of the aluminum crimp terminal 20 has an inner region 25 and an outer region 26 in a crimping recess facing portion 24 facing the crimping recess 23. The inner region 25 is in contact with the conductor 12 of the aluminum electric wire 10, and has an average crystal grain size of less than 50 μm. The outer region 26 is adjacent to the outside of the inner region 25, and has an average crystal grain size of 50 μm or more.

[0034] In the aluminum electric wire 1 with an aluminum crimp terminal, with the conductor 12 of the aluminum electric wire 10 inserted into the insertion portion 21 of the aluminum crimp terminal 20, force is applied to the insertion portion 21 from one direction to crimp the conductor 12 to the insertion portion 21. The cross-sectional shape of the conductor crimping portion 2 formed by applying force to the insertion portion 21 from one direction in this manner differs from the cross-sectional shape of the conductor crimping portion in a so-called compression terminal, in which force is applied to the insertion portion from multiple directions.

[0035] As described above, the conductor crimping portion 2 is formed by applying force from one direction to the insertion portion 21. When force is applied from one direction to the insertion portion 21, a portion of the insertion portion 21 is recessed. In a cross section of the conductor crimping portion 2, the crimping recess 23 is the recessed portion of the insertion portion 21. Also, as shown in FIG. 2, the crimping recess facing portion 24 is a portion that faces the crimping recess 23 across the conductor 12 in the insertion portion 21.

[0036] In the crimping recess facing portion 24, there are an inner region 25 and an outer region 26 from the inside to the outside of the insertion portion 21. The inner region 25, which is inside the insertion portion 21 and in contact with the conductive wire 12, has an average crystal grain size of less than 50 μm. The outer region 26, which is outside the insertion portion 21, has an average crystal grain size of 50 μm or more. Compared to the outer region 26, the inner region 25 has a smaller average crystal grain size.

[0037] 2, the cross-sectional shape of the insertion portion 21 before the conductor 12 and the insertion portion 21 are crimped is different from that of Fig. 2, and the crimping recess 23 is not formed. In the cross-sectional shape of the insertion portion 21 before crimping, the inner region 25 exists around the entire inner circumference of the insertion portion 21, and the outer region 26 exists around the entire outer circumference of the insertion portion 21. When the pre-crimped insertion portion 21 having the inner region 25 existing around the entire inner circumference and the outer region 26 existing around the entire outer circumference is crimped to the conductor 12 by receiving a force from one direction, the crystalline state of the insertion portion 21 before crimping is more likely to be maintained in the crimping recess facing portion 24 than in the crimping recess 23 of the conductor crimping portion 2.

[0038] Regarding the crimping mechanism between aluminum crimp terminal 20 having insertion portion 21 in such a crystalline state and aluminum electric wire 10 having conductor wire 12, the present inventors consider the following.

[0039] In the conductor crimping portion 2, the conductor 12 of the aluminum electric wire 10 and the insertion portion 21 of the aluminum crimp terminal 20 are crushed by a force from one direction and then joined by their mutual contact pressure (contact pressure). Here, in the deformation of an object, when an external force is removed, a force (elastic deformation) acts to return to the original shape. The direction of the elastic deformation differs between the conductor 12 and the insertion portion 21, causing contact pressure. This contact pressure may be weakened by a temperature rise when electricity is passed through the aluminum electric wire 10. This is thought to be because the movement of atoms constituting the material becomes more active due to a temperature rise, and the atomic arrangement is organized, thereby weakening the elastic deformation. Such a decrease in contact pressure is called stress relaxation. In general, the greater the amount of processing given to the insertion portion 21, the greater the rate of change in stress relaxation (stress relaxation rate).

[0040] The processing amount is the sum of the processing amount applied to the conductor 12 and the insertion portion 21 before crimping and the deformation amount applied by the crimping. When the processing amount applied to the conductor 12 before crimping and the processing amount applied to the insertion portion 21 before crimping are different, the stress relaxation rates due to the temperature rise are different from each other.

[0041] Furthermore, repeated switching between high and low temperature states by turning the current through the aluminum electric wire 10 on and off causes thermal expansion and contraction, which in turn causes a slight misalignment at the contact interface between the conductor 12 and the insertion portion 21. When a misalignment occurs, the oxide coating portion of the conductor 12 that had a natural oxide coating in the air before the misalignment comes into contact with the insertion portion 21, or the connection portion of the conductor 12 that was in contact with the insertion portion 21 before the misalignment separates from the insertion portion 21 and becomes non-contact, oxidizing in the air, which can increase the electrical resistance of the connection and further generate heat.

[0042] It was considered that if the stress relaxation rate of the conductor 12 and the stress relaxation rate of the insertion portion 21 differ during such thermal expansion and thermal contraction, the amount of minute slippage at the contact interface between the conductor 12 and the insertion portion 21 increases, and such amount of slippage contributes to the temperature rise of the aluminum electric wire 1 with aluminum crimp terminal. On the other hand, if the stress relaxation rate of the conductor 12 and the stress relaxation rate of the insertion portion 21 are the same or close to each other, the amount of minute slippage at the contact interface between the conductor 12 and the insertion portion 21 decreases during thermal expansion and thermal contraction, and the contact pressure is maintained, so that the temperature rise of the aluminum electric wire 1 with aluminum crimp terminal can be suppressed. Therefore, even if the aluminum electric wire 1 with aluminum crimp terminal is used for a long time, the increase in electrical resistance and heat generation are suppressed, and the aluminum electric wire 1 with aluminum crimp terminal can be used stably. Generally, for the conductor 12 of the aluminum electric wire 10 for power distribution lines, a hard material that has been processed to a large extent to increase the tensile strength in order to increase the breaking strength is used compared to pure aluminum.

[0043] For this reason, in order to make the processing amount of the insertion portion 21 close to the processing amount of the conductor 12, in addition to crimping the insertion portion 21 when crimping, the insertion portion 21 needs to be in a processed state (strongly processed state) before crimping. Specifically, it is required that the inner part of the insertion portion 21 that contacts the conductor 12 has a large residual strain so as not to cause a shift at the contact interface between the conductor 12 and the insertion portion 21.

[0044] Here, residual strain refers to strain caused by stress (residual stress) that exists within an object even after an external force has been removed, and is caused by disturbances in the crystal arrangement when looking at the metal structure microscopically. One evaluation index is the difference in crystal grain size, and the smaller the crystal grains are, the more crystal grain boundaries there are, which means that the crystal arrangement of the material as a whole is disturbed.

[0045] Therefore, if the average crystal grain size is less than 50 μm in the region around the entire inner circumference of insertion portion 21 before crimping, the residual strain will be large around the entire inner circumference of insertion portion 21, and the stress relaxation rate on the inside of insertion portion 21 will be the same as or close to the stress relaxation rate of conductor 12. As a result, even when aluminum electric wire 1 with aluminum crimp terminal is used for a long period of time, the contact pressure is maintained, so that the connection reliability of aluminum electric wire 1 with aluminum crimp terminal 1 is good, and increases in electrical resistance and heat generation are suppressed, allowing stable use of aluminum electric wire 1 with aluminum crimp terminal.

[0046] Therefore, the average crystal grain size of the inner region 25 is set to less than 50 μm. If the average crystal grain size of the inner region 25 is 50 μm or more, the change in contact pressure will be large, which may result in an increase in electrical resistance and heat generation. In addition, the average crystal grain size of the inner region 25 is preferably small in accordance with the amount of processing of the conductor 12, and specifically, is preferably less than 40 μm, and more preferably less than 30 μm.

[0047] In addition, in crimping the aluminum electric wire 10 and the aluminum crimp terminal 20, from the viewpoint of the workability of the worker at the construction site, it is required to hold the aluminum electric wire 10 in one hand and a crimping tool in the other hand to crimp the insertion part 21 of the aluminum crimp terminal 20. For this purpose, it is desired to reduce the force required for crimping the aluminum electric wire 10 and the aluminum crimp terminal 20 so that the connection reliability between the aluminum electric wire 10 and the aluminum crimp terminal 20 is good even when a light crimping tool is used. In general, the relationship between the crystal grain size and the hardness and strength of a material is expressed by the Hall-Petch formula, and the larger the crystal grain size, the softer the material. If the average crystal grain size is less than 50 μm from the inside to the outside of the insertion part 21, that is, in the entire region of the insertion part 21, the insertion part 21 itself becomes hard and the force required for crimping becomes large, resulting in poor workability.

[0048] Therefore, if the average crystal grain size is less than 50 μm in the entire inner circumferential region of insertion portion 21 before crimping and the average crystal grain size is 50 μm or more in the entire outer circumferential region of insertion portion 21 before crimping, the connection reliability of the aluminum electric wire 1 with an aluminum crimp terminal can be improved, such as by suppressing temperature rise after high-temperature endurance, and the force required for crimping the aluminum electric wire 10 and the aluminum crimp terminal 20 can be reduced. For this reason, the average crystal grain size of outer region 26 is set to 50 μm or more.

[0049] In addition, in the cross section of the conductor crimping portion 2, the ratio (h1 / (h1+h2))×100 of the thickness h1 of the inner region 25 to the total thickness (h1+h2) of the thickness h1 of the inner region 25 and the thickness h2 of the outer region is preferably 70% or less. The total thickness (h1+h2) of the thickness h1 of the inner region 25 and the thickness h2 of the outer region corresponds to the thickness h of the insertion portion 21 at the portion 24 facing the crimping recess. When the ratio (h1 / (h1+h2))×100 is 70% or less, the force required for crimping the aluminum electric wire 10 and the aluminum crimp terminal 20 can be further reduced, thereby further improving workability. When the ratio (h1 / (h1+h2))×100 is 30% or more, the connection reliability of the aluminum electric wire 1 with the aluminum crimp terminal can be improved, such as suppressing temperature rise after high-temperature endurance. From the above, in order to achieve both connection reliability and a reduction in the force required for crimping, the ratio (h1 / (h1+h2))×100 is preferably 30% or more and 70% or less.

[0050] Here, the measurement points for the thickness h of the crimping recess facing portion 24, the thickness h1 of the inner region 25, and the thickness h2 of the outer region 26 are specified as follows. As shown in Fig. 2, a straight line is drawn so that the convex portions on both sides of the crimping recess 23 are in contact with each other. A straight line S is drawn perpendicular to the line from midpoint A of the line whose two ends are the contact points of the convex portions on both sides toward the crimping recess facing portion 24. The length of the straight line S within the terminal region of the crimping recess facing portion 24 is defined as the thickness h of the crimping recess facing portion 24. Similarly, the length of the straight line S in the inner region 25 of the crimping recess facing portion 24 is defined as the thickness h1 of the inner region 25, and the length of the straight line S in the outer region 26 of the crimping recess facing portion 24 is defined as the thickness h2 of the outer region 26.

[0051] Moreover, the average Vickers hardness of the inner region 25 in the cross section of the conductor crimping portion 2 is preferably not less than 25. When the average Vickers hardness of the inner region 25 is not less than 25, the temperature rise of the aluminum electric wire 1 with an aluminum crimp terminal after endurance at high temperatures can be suppressed, and therefore the connection reliability between the aluminum electric wire 10 and the aluminum crimp terminal 20 is further improved.

[0052] Moreover, the average Vickers hardness of the inner region 25 in the cross section of the conductor crimping portion 2 is preferably 60 or less, more preferably 50 or less, and the average Vickers hardness of the outer region 26 in the cross section of the conductor crimping portion 2 is preferably less than 25. When the average Vickers hardness of the inner region 25 is 60 or less, the force required for crimping the aluminum electric wire 10 and the aluminum crimp terminal 20 can be further reduced, so that the workability is further improved, and when the average Vickers hardness of the inner region 25 is 50 or less, the workability is further improved. When the average Vickers hardness of the outer region 26 is less than 25, the force required for crimping the aluminum electric wire 10 and the aluminum crimp terminal 20 can be further reduced, so that the workability is further improved.

[0053] Furthermore, the difference between the average Vickers hardness of the inner region 25 and the average Vickers hardness of the outer region 26 in the cross section of the conductor crimping portion 2 is preferably 5 or more, and more preferably 10 or more. When the difference is 5 or more, a better balance is achieved between the effect of suppressing temperature rise after high-temperature endurance of the aluminum electric wire 1 with an aluminum crimp terminal, and the effect of reducing the force required to crimp the aluminum electric wire 10 and the aluminum crimp terminal 20. The measurement points for the Vickers hardness of the inner region 25 and the Vickers hardness of the outer region 26 are on the line S.

[0054] Next, a description will be given of a manufacturing method for the aluminum crimp terminal 20. The manufacturing method for the aluminum crimp terminal 20 mainly includes a first forging step S1, a heat treatment step S2, a second forging step S3, a punching step S4, and a plating step S5.

[0055] In the first forging process S1, the center of the aluminum round bar soft material is compressed by forging to form the insert part 21. The inside of the formed insert part 21 is processed and the material is significantly deformed, whereas the outside of the insert part 21 is relatively suppressed from deforming. When observed microscopically, the deformation of the material is the deformation of the crystal grains that constitute the material, so the crystal grain size becomes small over the entire inside circumference of the insert part 21. Furthermore, even if heat treatment is performed in the next process, the atoms in the area that is significantly deformed by processing are more likely to recrystallize due to the temperature during the heat treatment than the atoms in the area where deformation is suppressed, and a large number of recrystallized grains are formed. Therefore, the crystal grain size becomes small in the area that is significantly deformed, i.e., the inside of the insert part 21. In addition, after forging, the inside of the insert part may be machined to expand the diameter of the insert part, or the outside of the insert part may be machined.

[0056] The heat treatment step S2 carried out after the first forging step S1 has the effect of softening the entire aluminum crimp terminal 20 and homogenizing the structure. The heat treatment step S2 is not an essential step in the manufacturing method of the aluminum crimp terminal 20, but is an optional step.

[0057] In the second forging step S3 carried out after the heat treatment step S2, the end portion opposite to the insertion portion 21 is compressed by forging to form the shuttlecock portion 22 in a flat plate shape.

[0058] In the punching step S4 carried out after the second forging step S3, a through hole 22a is formed in the shuttlecock portion 22 by punching.

[0059] In the plating step S5 performed after the punching step S4, the aluminum crimp terminal 20 is plated. As an example, Ni-P plating is applied by double zincate treatment, Cu strike plating is applied on top of that to improve adhesion, and Sn plating is applied to the outermost layer. As another example, Cu plating is applied by double zincate treatment, and Sn plating is applied to the outermost layer. The double zincate treatment is a method of plating aluminum, in which zinc is plated first, and then the target plating is applied by replacing the zinc. In this way, the aluminum crimp terminal 20 is obtained.

[0060] Next, a description will be given of a method for producing the aluminum electric wire 1 with an aluminum crimp terminal. The method for producing the aluminum electric wire 1 with an aluminum crimp terminal mainly includes a compound insertion step S10 and a crimping step S12.

[0061] In the compound insertion step S10, a compound material is inserted into the insertion portion 21 to improve the adhesion between the conductor 12 and the insertion portion 21. The compound material is mainly composed of mineral oil and zinc powder, and is used to provide a good connection between the conductor 12 and the insertion portion 21. When the compound material is provided in the insertion portion 21, it plays a role in ensuring good conductivity of the aluminum electric wire 1 with aluminum crimp terminal, destroying the oxide coating of the conductor 12 and the oxide coating of the insertion portion 21, waterproofing the conductor crimp portion 2, etc.

[0062] In the crimping step S11 performed after the compound insertion step S10, the conductor 12 is inserted into the insertion portion 21, and a crimping tool is used to apply force to the insertion portion 21 from one direction to crimp the conductor 12 and the insertion portion 21. The crimping by applying force from one direction promotes deformation of the crystal grains inside the insertion portion 21 more than conventional compression, and the crystal grains become smaller in the inner region 25 of the crimping recess facing portion 24 on the opposite side to the crimping recess 23. The larger the depression amount of the crimping recess 23, which is the recessed portion of the insertion portion 21, in other words, the larger the pressing force during crimping, the smaller the crystal grains in the inner region 25 tend to become. In the cross section of the conductor crimping portion 2, the crimping depth d, which is expressed as the distance between the midpoint A on the crimping recess 23 side and the intersection point between the straight line S and the crimping recess 23, is preferably 5 mm or more.

[0063] Such an aluminum electric wire 1 with an aluminum crimp terminal is suitably used for electric wire end connections and electric wire connections in which good connection reliability is required between the aluminum electric wire 10 and the aluminum crimp terminal 20 even if the force for crimping the aluminum crimp terminal 20 is reduced.

[0064] According to the embodiment described above, by focusing on the structure of the insertion portion of the aluminum crimp terminal, in the cross section of the conductor crimping portion, the insertion portion of the aluminum crimp terminal has an inner region with an average crystal grain size of less than 50 μm and an outer region with an average crystal grain size of 50 μm or more, so that even if the force used to crimp the aluminum crimp terminal is reduced, the connection reliability between the aluminum electric wire and the aluminum crimp terminal is good.

[0065] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES

[0066] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.

[0067] (Examples 1 to 2, 4 to 6) The insertion part was formed by forging the center of a soft aluminum round bar with a diameter of 24 mm with the composition shown in Table 1. Next, in order to homogenize the structure of the sample that had been deformed by the forging process, a heat treatment was performed at 325°C for 2 hours. Next, the end opposite the insertion part was set in a previously prepared die and compression forged to form the shuttlecock part. Next, a through hole was opened in the shuttlecock part by punching. Next, Ni-P plating was applied by double zincate treatment, Cu strike plating was applied on top of that to improve adhesion, and Sn plating was applied to the outermost layer. Next, a compound material (Compound A, Furukawa Power Systems Co., Ltd.) was inserted into the insertion part to improve adhesion between the conductor and the insertion part. Next, a 100 mm long steel sheet with the composition shown in Table 1 was inserted. 2 The conductor wire was inserted into the insertion portion and crimped to a crimping depth d shown in Table 1 using a crimping tool (Izumi Seiki Seisakusho, REC-Li250M) to form a conductor crimped portion. In this way, an aluminum electric wire with an aluminum crimp terminal was obtained.

[0068] Example 3 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 1, except that no heat treatment was performed.

[0069] (Examples 7 to 8, Example 10) An aluminum electric wire with an aluminum crimp terminal was manufactured in the same manner as in Example 1, except that when forging was performed on the center part of the soft material of the aluminum round bar, an insertion part with a smaller diameter than that of Example 1 was formed, and then the inside of the insertion part was machined to adjust the thickness ratio of the region in the insertion part having an average crystal grain size of less than 50 μm to the region having an average crystal grain size of 50 μm or more, and the average crystal grain size, as shown in Table 1.

[0070] Example 9 An aluminum electric wire with an aluminum crimp terminal was manufactured in the same manner as in Example 1, except that a soft aluminum round bar that was 0.5 mm thicker than that in Example 1 was prepared, and an insertion portion of the same diameter as in Example 1 was formed when the center of the soft material was forged. The outside of the insertion portion was then machined to adjust the thickness ratio of the region in the insertion portion having an average crystal grain size of less than 50 μm to the region having an average crystal grain size of 50 μm or more, and the average crystal grain size, as shown in Table 1.

[0071] Example 11 When forging was performed on the center part of the soft material of the aluminum round bar, an insertion part with a smaller diameter than that of Example 1 was formed, and then the inside of the insertion part was machined to adjust the average crystal grain size and the thickness ratio of the region in the insertion part having an average crystal grain size of less than 50 μm to the region having an average crystal grain size of 50 μm or more as shown in Table 1. An aluminum electric wire with an aluminum crimp terminal was manufactured in the same manner as in Example 1, except that no heat treatment was performed.

[0072] Example 12 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 1, except that the homogenization heat treatment was performed at 100° C. for 2 hours.

[0073] Example 13 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 1, except that the homogenizing heat treatment was performed at 200° C. for 2 hours.

[0074] Example 14 The composition of the aluminum round bar is shown in Table 2. The diameter is 19 mm and the diameter is 60 mm. 2 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 5, except that the conductor wire was used.

[0075] Example 15 The composition of the aluminum round bar is shown in Table 3. The diameter is 27 mm. 2An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 1, except that the conductor wire was used.

[0076] Comparative Example 1 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Example 1, except that the insertion portion was formed by cutting the center of the soft material of the aluminum round bar.

[0077] Comparative Example 2 An aluminum electric wire with an aluminum crimp terminal was manufactured in the same manner as in Example 1, except that a soft aluminum tube having the composition shown in Table 1 was prepared, one end of the aluminum tube was used as the insertion portion, and the end opposite the insertion portion was pressed to form the shuttlecock portion.

[0078] Comparative Example 3 An aluminum electric wire with an aluminum crimp terminal was manufactured in the same manner as in Example 3, except that the insertion portion was formed by cutting the center of a hard aluminum round bar having a diameter of 24 mm and the composition shown in Table 1.

[0079] Comparative Example 4 The composition of the aluminum round bar is shown in Table 2. The diameter is 19 mm and the diameter is 60 mm. 2 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Comparative Example 1, except that the conductor wire was used and the crimping depth d was set to 6 mm.

[0080] Comparative Example 5 The composition of the aluminum round bar is shown in Table 3. The diameter is 27 mm. 2 An aluminum electric wire with an aluminum crimp terminal was produced in the same manner as in Comparative Example 1, except that the conductor wire was used.

[0081] [Measurement and Evaluation] The aluminum electric wires with aluminum crimp terminals obtained in the above Examples and Comparative Examples were subjected to the following measurements and evaluations. The results are shown in Tables 1 to 3. Fig. 3 shows an optical microscope photograph of a cross section of the conductor crimped portion constituting the aluminum electric wire with aluminum crimp terminal produced in Example 1.

[0082] [1] Average grain size First, a cross section perpendicular to the longitudinal direction of the aluminum electric wire was cut out from the conductor crimped portion of the aluminum electric wire with the aluminum crimp terminal. The cut sample was then filled with resin, and the sample surface was mirror-finished by wet polishing and buffing, after which electrolytic polishing and anodizing were performed. Next, the portion facing the crimped recess was photographed at 100x magnification using an optical microscope with a polarizing plate inserted.

[0083] Next, a straight line was drawn so that the convex portions on both sides of the crimping recess were in contact with each other. A straight line S was drawn perpendicular to the line from the midpoint A of the line with the contact points of the convex portions on both sides at both ends toward the crimping recess facing portion. The length of the straight line S in the terminal region of the crimping recess facing portion was taken as the thickness h of the crimping recess facing portion. Next, the thickness h of the crimping recess facing portion was divided into 10 equal parts, the number of intersections between the straight line S and the grain boundaries in each region was counted, and the length of the 10 equal parts of the thickness h was divided by the counted number to calculate the average crystal grain size of each region. The average crystal grain size of the inner region of the insertion portion was calculated by dividing the total value of the average crystal grain size of the regions having an average crystal grain size of less than 50 μm among these regions by the number of such regions. Similarly, the average crystal grain size of the outer region of the insertion portion was calculated by dividing the total value of the average crystal grain size of the regions having an average crystal grain size of 50 μm or more by the number of such regions.

[0084] [2] Average Vickers hardness value The sample on which the average crystal grain size was measured was pressed down for 15 seconds at a load of 50 gf in accordance with JIS Z2244, and the hardness was calculated from the length of the diagonal line of the indentation. This measurement was performed three times (n=3), and the average value was calculated as the average Vickers hardness. The measurement points were on the line S, at least four indentations away from the end of the insertion part or from the indentation that had already been measured.

[0085] [3] Temperature rise after heat cycle test To evaluate the temperature rise after high temperature durability, a heat cycle test was performed with reference to the heat cycle test described in "JIS C 2810 General Rules for Electric Wire Connectors for Indoor Wiring - Non-separable Type". Several aluminum electric wires with aluminum crimp terminals of 2m or more in length were prepared, and the terminals were connected in series via a terminal block, and the current value was set so that the temperature of the aluminum electric wire became 105°C. A slit was made in the insulating coating of the center part of any aluminum electric wire, and a thermocouple was inserted so that it contacted the conductor of the aluminum electric wire, and the temperature of the aluminum electric wire was measured. In addition, a thermocouple was soldered to the shuttlecock part of the aluminum terminal to measure the temperature of the aluminum terminal. The process of passing the current at the set current value for 1 hour and then stopping the current for 1 hour was defined as one cycle, and the temperature rise (°C) of the aluminum terminal after 500 cycles was measured compared to the temperature of the aluminum terminal after 25 cycles. If the temperature rise was less than 8°C, it was considered to have passed. The smaller the temperature rise, the better in terms of suppressing heat generation in the aluminum electric wire with aluminum crimp terminal.

[0086] [4] Crimping load In a test for evaluating the crimping force between the conductor of an aluminum electric wire and the insertion part of an aluminum crimp terminal, the conductor of an aluminum electric wire was inserted into the insertion part of the aluminum crimp terminal, and crimping dies (male, female, Izumi Seiki Seisakusho) were attached to the jig of a universal tensile tester (AG-100KND, manufactured by Shimadzu Corporation) to determine the load applied to the conductor crimped part when crimped to the crimping depth d shown in Tables 1 to 3. A crimping load of 75 kN or less was deemed to pass. The smaller the crimping load, the smaller the load when actually crimping the conductor and the insertion part, and the improved workability, so the crimping load is more preferably 65 kN or less, and more preferably 55 kN or less.

[0087] [Table 1]

[0088] [Table 2]

[0089] [Table 3]

[0090] As shown in Tables 1 to 3, in the cross section of the conductor crimping portion, the insertion portion of the aluminum crimp terminal had an inner region having an average crystal grain size of less than 50 μm and an outer region having an average crystal grain size of 50 μm or more in Examples 1 to 15. Therefore, the suppression of temperature rise and the reduction of crimping load after the heat cycle test were well balanced. In particular, in Examples 1 to 2, 4 to 5, 7 to 8, 10, and 13 to 15, the ratio (h1 / (h1+h2))×100 of the thickness h1 of the inner region, the average value of the Vickers hardness of the inner region, and the average value of the Vickers hardness of the outer region were within the suitable ranges, so the suppression of temperature rise and the reduction of the crimping load after the heat cycle test were even better.

[0091] On the other hand, in Comparative Examples 1-2 and 4-5, the inserting portion of the aluminum crimp terminal did not have an inner region having an average crystal grain size of less than 50 μm, so the temperature rise after the heat cycle test was large. Also, in Comparative Example 3, the inserting portion of the aluminum crimp terminal did not have an outer region having an average crystal grain size of 50 μm or more, so the crimping load was large. [Explanation of symbols]

[0092] 1 Aluminum wire with aluminum crimp terminal 2 Conductor crimping section 10. Aluminum wire 11 Wire 12 Conductor 13 Insulating coating 14 Sheath 20 Aluminum crimp terminal 21 Insertion section 22 Battledore Club 22a Through hole 23 Crimping recess 24 Crimping recess facing part 25 Inner area 26 Outer area

Claims

1. An aluminum electric wire with an aluminum crimp terminal, the aluminum electric wire having a conductor crimping portion in which a conductor of the aluminum electric wire is crimped into a tubular insertion portion of the aluminum crimp terminal, The composition of the conductor is A1070, The aluminum crimp terminal has a composition of A1050 or A1070, In a cross section of the conductor crimping portion perpendicular to the longitudinal direction of the aluminum electric wire, The insertion portion of the aluminum crimp terminal has, at a crimp recess facing portion facing the crimp recess, an inner region that contacts the conductor of the aluminum electric wire and has an average crystal grain size of 10 μm or more and 35 μm or less, and an outer region that is adjacent to the outside of the inner region and has an average crystal grain size of 80 μm or more and 120 μm or less, A ratio (h1 / (h1+h2))×100 of the thickness h1 of the inner region to the total thickness (h1+h2) of the thickness h1 of the inner region and the thickness h2 of the outer region is 10% or more and 70% or less.

1. An aluminum electric wire with an aluminum crimp terminal.

2. 2. The aluminum electric wire with aluminum crimp terminal according to claim 1, wherein an average Vickers hardness value of the inner region in the cross section is 25 or more.

3. 3. The aluminum electric wire with aluminum crimp terminal according to claim 1, wherein an average Vickers hardness of the inner region in the cross section is 50 or less, and an average Vickers hardness of the outer region in the cross section is less than 25.

Citation Information

Patent Citations

  • JP1975001409U

  • Terminal and electric wire including the same

    JP2019169364A

  • Terminal-equipped wire

    JP2020027758A