Method for producing optically anisotropic film
By integrating photo-alignment and magnetic field alignment techniques, the method ensures a uniform tilt angle of liquid crystal compounds in optically anisotropic films, addressing the issue of inconsistent tilt angles in existing manufacturing methods.
Patent Information
- Application Number
- JP2022539488
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-26
- Filing Date
- 2021-07-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Existing methods for manufacturing optically anisotropic films using liquid crystal compounds result in inconsistent tilt angles of the liquid crystal compound near the base material interface, leading to continuous changes in tilt angle along the thickness direction.
A method combining photo-alignment film alignment and magnetic field alignment is used to control the tilt angle of a polymerizable liquid crystal compound, involving steps of applying a photo-alignment composition, irradiating with oblique ultraviolet light, coating a liquid crystal composition, applying a magnetic field, and curing the layer.
The method achieves a constant tilt angle of the liquid crystal compound throughout the thickness direction, ensuring uniform orientation and alignment.
Smart Images

Figure 0007559069000008 
Figure 0007559069000009 
Figure 0007559069000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an optically anisotropic film having a uniform tilt orientation in the thickness direction. [Background technology]
[0002] Optically anisotropic films formed using liquid crystal compounds are used not only in image display devices such as optical compensation sheets and retardation films, but in recent years, their applications have expanded to include communication devices, cameras, and optical components for AR / VR.
[0003] In these fields, optically anisotropic films are becoming thicker, and in addition to the conventional liquid crystal alignment control methods using rubbing treatment and photoalignment treatment, alignment control techniques using magnetic fields have been researched.
[0004] For example, Patent Document 1 discloses a method for producing an optically anisotropic film in which the optical axis of a liquid crystal compound is tilted using a magnetic field. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4378910 Summary of the Invention [Problem to be solved by the invention]
[0006] The present inventors have studied the manufacturing method described in Patent Document 1 and have found that there is a problem in that the tilt control of the liquid crystal compound in the vicinity of the substrate interface is insufficient, and the tilt angle changes continuously along the thickness direction.
[0007] Therefore, an object of the present invention is to provide a method for producing an optically anisotropic film in which the tilt angle of a liquid crystal compound is controlled to be constant in the thickness direction. [Means for solving the problem]
[0008] As a result of intensive research to achieve the above-mentioned object, the inventors have discovered that by combining alignment control by a photo-alignment film and alignment control by application of a magnetic field, the tilt angle of a liquid crystal compound can be made uniform in the thickness direction of an optically anisotropic film, and have completed the present invention. That is, it has been found that the above object can be achieved by the following configuration.
[0009] (1) A method for producing an optically anisotropic film using a liquid crystal composition containing a polymerizable liquid crystal compound having magnetic field responsiveness, comprising the steps of: Step 1 of applying a photoalignment composition onto a substrate to form a photoalignment composition layer; A step 2 of irradiating the surface of the photoalignment composition layer with unpolarized and collimated ultraviolet light from an oblique direction; A step 3 of applying a liquid crystal composition onto the photoalignment composition layer irradiated with ultraviolet light to form a liquid crystal composition layer; Step 4 of applying a magnetic field to the liquid crystal composition layer in a direction substantially parallel to the direction of irradiation with the ultraviolet light in step 2 at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state; and step 5 of curing the liquid crystal composition layer in this order. (2) The method for producing an optically anisotropic film according to (1), wherein in step 2, the irradiation direction of the ultraviolet ray is at an angle of 5 to 85° with respect to the normal direction of the surface of the photoalignment composition layer. (3) The method for producing an optically anisotropic film according to (1) or (2), wherein the polymerizable liquid crystal compound is a rod-shaped liquid crystal compound having three or more benzene rings. (4) The method for producing an optically anisotropic film according to any one of (1) to (3), wherein in step 4, the magnetic field has a magnetic flux density of 0.2 to 1.0 T. Effect of the Invention
[0010] According to the present invention, there can be provided a method for producing an optically anisotropic film in which the tilt angle of a liquid crystal compound is controlled to be constant in the thickness direction. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram for explaining step 1. [Diagram 2] FIG. 13 is a diagram for explaining step 2. [Diagram 3] FIG. 11 is a diagram for explaining step 3. [Figure 4] FIG. 11 is a diagram for explaining step 4. [Diagram 5] FIG. 2 is a diagram for explaining a cross-sectional slice. [Figure 6] FIG. 13 is a diagram for explaining the area of a cross-sectional slice. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. In this specification, a numerical range indicated using "~" means a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in a certain numerical range. In addition, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0013] In this specification, the amount of each component in a composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. As used herein, a combination of two or more preferred embodiments is a more preferred embodiment. In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0014] The manufacturing method of the present disclosure will be described in detail below. The method for producing the optically anisotropic film of the present invention includes the following steps 1 to 5 in this order. Step 1: Applying a photoalignment composition onto a substrate to form a photoalignment composition layer Step 2: A step of irradiating the surface of the photoalignment composition layer with unpolarized and collimated ultraviolet light from an oblique direction. Step 3: A step of applying a liquid crystal composition containing a polymerizable liquid crystal compound having magnetic field responsiveness onto the photoalignment composition layer irradiated with ultraviolet light to form a liquid crystal composition layer. Step 4: applying a magnetic field to the liquid crystal composition layer in a direction substantially parallel to the direction of irradiation with the ultraviolet light in step 2 at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state. Step 5: Curing the liquid crystal composition layer Each step will be described below with reference to the drawings.
[0015] <Process 1> Step 1 is a step of applying a photo-alignment composition onto a substrate to form a photo-alignment composition layer. By carrying out step 1, a photo-alignment composition layer 12 is disposed on a substrate 10 as shown in FIG. In the following, first, the materials used in step 1 will be described in detail, and then the steps of the step will be described in detail.
[0016] (base material) The type of the substrate is not particularly limited as long as it is a member that supports the photoalignment composition layer. Examples of the substrate include a glass plate, a quartz plate, and a polymer film, with a glass plate being preferred. The thickness of the substrate is not particularly limited, but is preferably 0.1 to 4 mm, and more preferably 0.5 to 2 mm.
[0017] (Photoalignment composition) The photoalignment composition includes a photoalignment compound. The photoalignment compound is a compound having a photoalignment group. The photo-alignable group is a functional group that can impart anisotropy to the film by light irradiation. More specifically, it is a group that can cause a change in the molecular structure in the group by light (e.g., linearly polarized light) irradiation. Typically, it refers to a group that causes at least one photoreaction selected from photoisomerization reaction, photodimerization reaction, and photodecomposition reaction by light (e.g., linearly polarized light) irradiation. Among these photo-alignable groups, groups that undergo a photoisomerization reaction (groups having a photoisomerizable structure) and groups that undergo a photodimerization reaction (groups having a photodimerizable structure) are preferred, and groups that undergo a photodimerization reaction are more preferred.
[0018] The group that undergoes the above-mentioned photoisomerization reaction is preferably a group that contains a C=C bond or an N=N bond and undergoes a photoisomerization reaction. Examples of such groups include a group having an azobenzene structure (skeleton), a group having a hydrazono-β-ketoester structure (skeleton), a group having a stilbene structure (skeleton), and a group having a spiropyran structure (skeleton). Examples of groups that undergo the photodimerization reaction include groups having a cinnamic acid (cinnamoyl) structure (skeleton), groups having a coumarin structure (skeleton), groups having a chalcone structure (skeleton), groups having a benzophenone structure (skeleton), and groups having an anthracene structure (skeleton).
[0019] Examples of the photoalignment compound include those described in JP-A-2006-285197, JP-A-2007-076839, JP-A-2007-138138, JP-A-2007-094071, JP-A-2007-121721, JP-A-2007-140465, JP-A-2007-156439, JP-A-2007-133184, and JP-A-2007-140465. azo compounds described in JP-A-2009-109831, JP-A-3883848 and JP-A-4151746, aromatic ester compounds described in JP-A-2002-229039, maleimide and / or alkenyl-substituted esters having photo-alignable units described in JP-A-2002-265541 and JP-A-2002-317013 Examples of the photo-crosslinkable silane derivatives include nadimide compounds, photo-crosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, photo-crosslinkable polyimides, photo-crosslinkable polyamides, and photo-crosslinkable polyesters described in JP-T-2003-520878, JP-T-2004-529220, and JP-T-4162850, and photo-dimerizable compounds described in JP-A-9-118717, JP-T-10-506420, JP-T-2003-505561, WO2010 / 150748, JP-A-2013-177561, and JP-A-2014-012823. In particular, cinnamate compounds, chalcone compounds, and coumarin compounds are exemplified as preferred examples. Among these, azo compounds, photocrosslinkable polyimides, photocrosslinkable polyamides, photocrosslinkable polyesters, cinnamate compounds, and chalcone compounds are preferably used.
[0020] The photoalignment composition preferably contains a solvent. The solvent includes water and organic solvents. Examples of organic solvents include ketones, ethers, aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, halogenated carbons, esters, alcohols, cellosolves, cellosolve acetates, sulfoxides, and amides. These may be used alone or in combination of two or more.
[0021] The photoalignment composition may contain other components in addition to those described above, such as an adhesion improver, a leveling agent, a surfactant, and a plasticizer.
[0022] (Step 1) In step 1, the method for applying the photoalignment composition onto the substrate is not particularly limited. Coating methods include, for example, spin coating, die coating, gravure coating, flexographic printing, and inkjet printing.
[0023] After the photoalignment composition is applied onto the substrate, a drying treatment may be carried out, if necessary. The drying treatment may be a heat treatment. The conditions for the heat treatment are not particularly limited, but the heating temperature is preferably 30 to 100° C., and the heating time is preferably 10 to 600 seconds.
[0024] By the above procedure, a photoalignment composition layer is formed on the substrate. There is no limitation on the thickness of the photoalignment composition layer, and the thickness may be appropriately set so as to obtain the necessary alignment function depending on the photoalignment compound. The thickness of the photoalignment composition layer is preferably from 0.01 to 5 μm, and more preferably from 0.05 to 2 μm.
[0025] <Process 2> Step 2 is a step of irradiating the surface of the photo-alignment composition layer with unpolarized and collimated ultraviolet light from an oblique direction. As shown in Fig. 2, the surface of the photo-alignment composition layer 12 is irradiated with unpolarized and collimated ultraviolet light from an oblique direction as shown by the white arrow. Note that the oblique direction refers to a direction tilted by an angle of θ1 degrees with respect to the normal direction of the surface of the photo-alignment composition layer 12, as shown in Fig. 2. By carrying out the above step 2, an alignment control force is imparted to the surface of the photoalignment composition layer. That is, a photoalignment composition layer capable of controlling the alignment direction of the liquid crystal compound disposed on the surface is formed. The procedure for step 2 is described in detail below.
[0026] As described above, in step 2, the photoalignment composition layer is irradiated with a predetermined ultraviolet ray from an oblique direction. As described above, the "oblique direction" is not particularly limited as long as it is a direction inclined at a polar angle θ1 (0<θ<90°) with respect to the normal direction of the surface of the photoalignment composition layer, and can be appropriately selected depending on the purpose. In particular, the irradiation direction of the ultraviolet light is preferably 5 to 85°, more preferably 20 to 80°, relative to the normal direction of the surface of the photoalignment composition layer. That is, θ1 in FIG.
[0027] The photoalignment composition layer is irradiated with unpolarized and collimated ultraviolet light. The ultraviolet light includes light having a wavelength of 10 to 400 nm. Unpolarized light is random light with no particular observed dominant polarization state. The concept of collimated light includes not only completely parallel light, but also substantially parallel light (for example, some converging light and some diverging light). More specifically, the parallelism of collimated light is preferably within ±15°, more preferably within ±10°, and even more preferably within ±5°. Examples of light sources for irradiating the ultraviolet rays include xenon lamps, high-pressure mercury lamps, extra-high-pressure mercury lamps, and metal halide lamps. By using an interference filter or a color filter on the light obtained from such a light source, the wavelength range of the light to be irradiated can be limited. Furthermore, by using a collimating lens or louver for the light from these light sources, collimated light can be obtained.
[0028] The integrated amount of ultraviolet light is not particularly limited as long as it can impart the alignment control ability to the liquid crystal molecules to the photoalignment composition layer, but is preferably 10 to 3000 mJ / cm. 2 is preferable, and 500 to 2000 mJ / cm 2 is more preferred. The illuminance of the ultraviolet light is not particularly limited as long as it can impart the alignment control ability to the liquid crystal molecules to the photoalignment composition layer, but is preferably 1 to 300 mW / cm. 2 is preferable, and 5 to 100 mW / cm 2 is more preferred.
[0029] <Process 3> In step 3, a liquid crystal composition containing a polymerizable liquid crystal compound having magnetic field responsiveness is applied onto the photoalignment composition layer irradiated with ultraviolet light to form a liquid crystal composition layer. By carrying out step 3, a laminate including a substrate 10, a photoalignment composition layer 12, and a liquid crystal composition layer 14 is formed. In the following, we will first describe in detail the materials used in step 3, and then describe the steps of the step.
[0030] (Liquid crystal composition) The liquid crystal composition contains a polymerizable liquid crystal compound that is responsive to a magnetic field. The polymerizable liquid crystal compound having magnetic field responsiveness is a polymerizable liquid crystal compound that changes its orientation direction in response to a magnetic field applied in step 4 described below. More specifically, when the polymerizable liquid crystal compound has a mesogen group containing multiple aromatic ring structures, it has excellent magnetic field responsiveness. The mesogen group is a group that represents the main skeleton of the liquid crystal molecule that contributes to the formation of liquid crystal. The aromatic ring structure may be a monocyclic aromatic ring structure or a polycyclic aromatic ring structure. Examples of the aromatic ring structure include a benzene ring structure and a naphthalene ring structure. The aromatic ring structures included in the mesogenic group may be directly bonded to each other, or may be bonded to each other via a divalent linking group other than the aromatic ring structure (for example, -CO-, -O-, -NR- (R represents a hydrogen atom or an alkyl group), or a divalent aliphatic group).
[0031] The polymerizable liquid crystal compound having magnetic field responsiveness preferably has a mesogen group represented by formula (X). Formula (X) - (ZL) n - Z represents a divalent aromatic ring group or a divalent aliphatic ring group. L represents a single bond or a divalent linking group other than a divalent aromatic ring group and a divalent aliphatic ring group. n represents an integer of 2 or more. However, the mesogenic group represented by formula (X) contains two or more divalent aromatic ring groups.
[0032] The divalent aromatic ring group may have a monocyclic structure or a polycyclic structure. An example of the divalent aromatic ring group is a phenylene group. The divalent aromatic ring group may be condensed with a non-aromatic ring, for example, a phenylene group may be condensed with a non-aromatic ring containing a hetero atom. An example of the divalent aliphatic ring group is a cyclohexylene group.
[0033] Examples of the divalent linking group other than a divalent aromatic ring group and a divalent aliphatic ring group represented by L include -COO-, -CO-, -O-, -S-, -CONR 1 -, -SO2-, and -NR 2 - and others. R 1 ~R 2 each independently represents a hydrogen atom or an alkyl group.
[0034] n represents an integer of 2 or more, preferably an integer of 2 to 5, and more preferably an integer of 2 to 4.
[0035] The polymerizable liquid crystal compound having magnetic field responsiveness has a polymerizable group. The type of polymerizable group is not particularly limited, and examples thereof include unsaturated polymerizable groups, epoxy groups, and aziridinyl groups. An unsaturated polymerizable group is preferred, an ethylenically unsaturated polymerizable group is more preferred, and an acryloyl group or methacryloyl group is even more preferred. The polymerizable group can be introduced into the molecule of the liquid crystal compound by various methods. The polymerizable liquid crystal compound preferably has 1 to 6 polymerizable groups, and more preferably has 1 to 3 polymerizable groups.
[0036] As the polymerizable liquid crystal compound having magnetic field responsiveness, a compound represented by formula (Y) is preferable. Formula (Y) P 1 -L 1 -ML 2 -P 2 P 1 and P 2 each independently represents a polymerizable group. The polymerizable group is defined as above. L 1 and L 2 each independently represents a divalent linking group. Examples of the divalent linking group include a divalent hydrocarbon group (for example, a divalent aliphatic hydrocarbon group such as an alkylene group having 1 to 10 carbon atoms, an alkenylene group having 1 to 10 carbon atoms, and an alkynylene group having 1 to 10 carbon atoms, and a divalent aromatic hydrocarbon group such as an arylene group), a divalent heterocyclic group, -O-, -S-, -NH-, -N(Q)-, -CO-, or a group combining these (for example, an -O-divalent hydrocarbon group-, -(O-divalent hydrocarbon group) m -O- (m is an integer of 1 or more), and a divalent hydrocarbon group -O-CO-, etc. Q represents a hydrogen atom or an alkyl group. M represents a mesogenic group represented by formula (X).
[0037] As the polymerizable liquid crystal compound having magnetic field responsiveness, a rod-shaped polymerizable liquid crystal compound is preferable, and among them, a rod-shaped liquid crystal compound having three or more benzene rings is more preferable. Examples of rod-shaped polymerizable liquid crystal compounds include rod-shaped nematic liquid crystal compounds.Preferred rod-shaped nematic liquid crystal compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only low molecular weight liquid crystal compounds but also high molecular weight liquid crystal compounds can be used.
[0038] Examples of the polymerizable liquid crystal compound include compounds described in Makromol.Chem., Vol. 190, p. 2255 (1989), Advanced Materials, Vol. 5, p. 107 (1993), U.S. Pat. Nos. 4,683,327, 5,622,648, and 5,770,107, WO95 / 022586, WO95 / 024455, WO97 / 00600, WO98 / 023580, and WO98 / 052905, JP-A-1-272551, JP-A-6-016616, JP-A-7-110469, JP-A-11-080081, and JP-A-2001-328973. Two or more kinds of polymerizable liquid crystal compounds may be used in combination. When two or more kinds of polymerizable liquid crystal compounds are used in combination, the alignment temperature can be lowered.
[0039] The liquid crystal composition may contain a solvent. The solvent includes water and organic solvents. Examples of the organic solvent include the solvents exemplified as the organic solvent that may be contained in the photoalignment composition described above.
[0040] The liquid crystal composition may contain other components in addition to those described above, such as an adhesion improver, a leveling agent, a surfactant, and a plasticizer.
[0041] (Step 3) In step 3, the method for applying the liquid crystal composition onto the photoalignment composition layer is not particularly limited. Coating methods include, for example, spin coating, die coating, gravure coating, flexographic printing, and inkjet printing.
[0042] After the liquid crystal composition is applied onto the photoalignment composition layer, a drying treatment may be carried out, if necessary. The drying treatment may be a heat treatment. The conditions for the heat treatment are not particularly limited, but the heating temperature is preferably 30 to 150° C., and the heating time is preferably 10 to 600 seconds.
[0043] By the above procedure, a liquid crystal composition layer is formed on the photoalignment composition layer. There is no limitation on the thickness of the liquid crystal composition layer, and the thickness may be appropriately set so as to obtain the necessary alignment function depending on the type of polymerizable liquid crystal compound. The thickness of the photoalignment composition layer is preferably from 5 to 100 μm, and more preferably from 20 to 50 μm.
[0044] After step 3 and before step 4 described below, a step of subjecting the liquid crystal composition layer to a heat treatment to align the liquid crystal compound in the liquid crystal composition layer may be carried out. The temperature for the heat treatment may be a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state.
[0045] <Step 4> Step 4 is a step of applying a magnetic field to the liquid crystal composition layer in a direction substantially parallel to the direction of ultraviolet irradiation in step 2 at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state. In step 4, as shown by the black arrow in Fig. 4, a magnetic field is applied to the liquid crystal composition layer 14 in a direction substantially parallel to the direction of ultraviolet irradiation in step 2. Note that, as shown in Fig. 4, the direction in which the magnetic field is applied is inclined by θ2 degrees with respect to the normal direction to the surface of the liquid crystal composition layer 14, and θ2 degrees shown in Fig. 4 represents the same angle as θ1 degree shown in Fig. 2. The procedure for step 4 is described in detail below.
[0046] Step 4 is performed at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state, that is, step 4 is performed in a temperature range at which the liquid crystal composition in the liquid crystal composition layer exhibits a liquid crystal phase. The above temperature is preferably equal to or higher than the liquid crystal transition temperature of the polymerizable liquid crystal compound contained in the liquid crystal composition layer.
[0047] The direction in which the magnetic field is applied is substantially parallel to the direction of ultraviolet light irradiation in step 2. "Substantially parallel" means that the angle between the direction in which the magnetic field is applied and the direction of ultraviolet light irradiation is within 7°, and preferably within 3°.
[0048] The magnetic flux density of the magnetic field is preferably 0.1 T or more, more preferably 0.2 T or more, and further preferably 0.4 T or more. From the viewpoint of productivity, the upper limit is preferably 2.0 T or less, and more preferably 1.0 T or less. The application time of the magnetic field is not particularly limited, but is preferably 10 minutes or less, and from the viewpoint of productivity, more preferably 1 minute or less.
[0049] The method for applying the magnetic field is not particularly limited, and examples thereof include a method using a permanent magnet or an electromagnet. A magnetic field may be simultaneously applied to the entire liquid crystal composition layer having a large area by using a plurality of magnets. Alternatively, a magnetic field may be applied by conveying a substrate having a liquid crystal composition layer laminated thereon in a region where a magnetic field is generated in a certain direction.
[0050] After the above step 4, a step of lowering the temperature from the temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state may be performed while the magnetic field is being applied to the liquid crystal composition layer. By performing the above step, the temperature of the liquid crystal composition layer is lowered to a temperature lower than the temperature at which the liquid crystal composition exhibits an aligned state. The temperature of the liquid crystal composition layer is preferably lowered to room temperature (25° C.).
[0051] <Process 5> Step 5 is a step of curing the liquid crystal composition layer obtained in step 4. The method of the curing treatment is not particularly limited, and examples thereof include light irradiation treatment and heat treatment. Among them, from the viewpoint of manufacturability, light irradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. The irradiation conditions for the light irradiation treatment are not particularly limited, but are preferably 50 to 1000 mJ / cm 2 is preferred. The light irradiation is preferably carried out at room temperature (25° C.).
[0052] When the light irradiation process is performed, the light irradiation may be performed all at once, or the illuminance may be changed and the light irradiation may be performed stepwise. When the light irradiation is performed stepwise by changing the irradiation, it is preferable to perform the light irradiation stepwise while increasing the illuminance. For example, the light irradiation may be performed at a temperature of 20 mW / cm. 2 Less than or equal to 15mW / cm 2 After the first light irradiation at an illuminance of 20 mW / cm 2 More than (preferably 50mW / cm 2 A second light irradiation may be performed at an illuminance of 100 nm or more.
[0053] By carrying out the above steps, an optically anisotropic film is produced in which the tilt angle of the liquid crystal compound is controlled to be constant in the thickness direction. The thickness of the optically anisotropic film is not particularly limited, and is preferably from 5 to 100 μm, more preferably from 20 to 50 μm.
[0054] There is no limitation on the front retardation of the optically anisotropic film at a wavelength of 550 nm, and the retardation that provides the required alignment function may be appropriately set. The front retardation at a wavelength of 550 nm is preferably from 1000 to 10000 nm, and more preferably from 3000 to 6000 nm. It is most preferable that the retardation film has reverse dispersion, but a retardation plate having small wavelength dispersion of retardation or a liquid crystal cured film having normal dispersion can also be used. Note that reverse dispersion means that the absolute value of retardation increases with increasing wavelength, and normal dispersion means that the absolute value of retardation increases with decreasing wavelength.
[0055] <Application> The optically anisotropic film produced by the production method of the present invention can be used as a color-eliminating film for image display devices, a beam splitter for laser light sources, a low-pass filter for imaging, and the like. EXAMPLES
[0056] Hereinafter, the present disclosure will be described more specifically with reference to examples. However, the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.
[0057] <Example 1> (Formation of photo-alignment composition layer (Step 1)) A glass plate was prepared as a support. The following photo-alignment composition was applied to the support by spin coating to form a photo-alignment composition layer. The support on which the photo-alignment composition layer was formed was dried on a hot plate at 60° C. for 60 seconds.
[0058] ───────────────────────────────── photoalignment composition ------------------------------------------------------------------ 1.00 parts by mass of the following photoalignment compound Water 16.00 parts by mass Butoxyethanol 42.00 parts by weight Propylene glycol monomethyl ether 42.00 parts by mass ------------------------------------------------------------------
[0059] photo alignment compound
[0060] [ka]
[0061] (Exposure of photoalignment composition layer (step 2)) The obtained photoalignment composition layer was irradiated with collimated unpolarized ultraviolet light at an angle of 45° to the normal direction of the film surface (2000 mJ / cm 2 The photoalignment composition layer was exposed to light by using a super-high pressure mercury lamp and a collimating lens.
[0062] (Formation of Liquid Crystal Composition Layer (Step 3)) The following liquid crystal composition A-1 was prepared as a liquid crystal composition: This liquid crystal composition A-1 is a liquid crystal composition that forms nematic liquid crystals. ───────────────────────────────── Liquid crystal composition A-1 ───────────────────────────────── 100.00 parts by mass of the following rod-shaped liquid crystal compound L-1 Polymerization initiator (Omnirad819, manufactured by BASF) 4.00 parts by mass 1.00 parts by mass of HYSOLV MTEM (manufactured by Toho Chemical Industry Co., Ltd.) Cyclopentanone 171.12 parts by mass ─────────────────────────────────
[0063] Rod-shaped liquid crystal compound L-1 (a mixture of the following compounds. All of the compounds are polymerizable liquid crystal compounds that are responsive to magnetic fields.)
[0064] [ka]
[0065] The liquid crystal composition A-1 was applied onto the exposed photoalignment composition layer, and the resulting coating was heated on a hot plate to 110°C to dry the solvent, obtaining a liquid crystal composition layer. Thereafter, while maintaining the temperature at 110°C with hot air, a magnetic field (0.6T) was applied from a direction of 45° to the normal direction of the liquid crystal composition layer using an electromagnet. The temperature of 110° C. was the temperature at which the liquid crystal composition in the liquid crystal composition exhibited a liquid crystal phase. The direction of the applied magnetic field was parallel to the direction of the irradiation of the ultraviolet light. The specimen was cooled to 25°C with a magnetic field applied, and exposed to an air atmosphere with an illumination intensity of 10 mW / cm 2 UV irradiation (100mJ / cm 2 The alignment of the liquid crystal compound was fixed by irradiating the liquid crystal molecules with a 365 nm LED (UV wavelength). The liquid crystal molecules were then irradiated with a 100 mW / cm illuminance under a nitrogen atmosphere. 2 UV irradiation (300 mJ / cm 2 The polymerization was completed by irradiating the light with UV light (LED-UV wavelength 365 nm) to obtain an optically anisotropic film. The thickness of the obtained optically anisotropic film was 31.1 μm. Furthermore, the retardation measurements at a wavelength of 550 nm at incident angles of -45°, 0°, and 45° (on a plane including the direction of the magnetic field application) using Axometrix's AxoScan were 850 nm, 2550 nm, and 5200 nm. Since the retardation at -45° and 45° was different, it was confirmed that the liquid crystal molecules were tilted relative to the film surface.
[0066] <Examples 2 to 4> Optically anisotropic films were prepared in the same manner as in Example 1, except that the thickness of the liquid crystal composition layer and the magnetic flux density were changed.
[0067] <Example 5> An optically anisotropic film was produced in the same manner as in Example 1, except that the following liquid crystal composition A-2 was used as the liquid crystal composition. ───────────────────────────────── Liquid crystal composition A-2 ───────────────────────────────── 50.00 parts by mass of the following rod-shaped liquid crystal compound L-2 50.00 parts by mass of the following rod-shaped liquid crystal compound L-3 Polymerization initiator (Omnirad819, manufactured by BASF) 4.00 parts by mass 1.00 parts by mass of HYSOLV MTEM (manufactured by Toho Chemical Industry Co., Ltd.) Cyclopentanone 171.12 parts by mass ─────────────────────────────────
[0068] Rod-shaped liquid crystal compound L-2 (corresponding to a polymerizable liquid crystal compound having magnetic field responsiveness)
[0069] [ka]
[0070] Rod-shaped liquid crystal compound L-3 (corresponding to a polymerizable liquid crystal compound having magnetic field response)
[0071] [ka]
[0072] <Comparative Example 1> Irradiate with non-collimated, polarized UV light (2000 mJ / cm 2 An optically anisotropic film was produced in the same manner as in Example 1, except that a super-high pressure mercury lamp was used. The direction of the magnetic field was parallel to a plane including the amplitude direction of the polarized ultraviolet light.
[0073] <Comparative Example 2> An optically anisotropic film was produced in the same manner as in Example 1, except that no magnetic field was applied during aging.
[0074] <Comparative Example 3> An optically anisotropic film was produced in the same manner as in Example 1, except that the following liquid crystal composition A-3 was used as the liquid crystal composition. ───────────────────────────────── Liquid crystal composition A-3 ───────────────────────────────── 50.00 parts by mass of the following rod-shaped liquid crystal compound L-4 50.00 parts by mass of the following rod-shaped liquid crystal compound L-5 Polymerization initiator (Omnirad819, manufactured by BASF) 4.00 parts by mass 1.00 parts by mass of HYSOLV MTEM (manufactured by Toho Chemical Industry Co., Ltd.) Cyclopentanone 171.12 parts by mass ─────────────────────────────────
[0075] Rod-shaped liquid crystal compound L-4 (not a polymerizable liquid crystal compound with magnetic field response)
[0076] [ka]
[0077] Rod-shaped liquid crystal compound L-5 (not a polymerizable liquid crystal compound with magnetic field response)
[0078] [ka]
[0079] (Evaluation method) After peeling off the optically anisotropic film from the glass substrate, a cross-sectional slice was prepared using a microtome, and the cross-sectional slice was placed on a slide glass. When preparing the cross-sectional slice, the optically anisotropic film was observed from the normal direction, and cut along the direction in which the liquid crystal compound was oriented to prepare the cross-sectional slice. More specifically, as shown in FIG. 5, in the optically anisotropic film 16, the liquid crystal compound was oriented in the y direction when observed from the normal direction, so that the cross-sectional slice 18 was obtained by cutting along the y direction. As shown in FIG. 5, the side 18E of the cross-sectional slice 18 corresponds to the side in the thickness direction of the optically anisotropic film 16. The cross-sectional piece prepared above was placed between two polarizing plates arranged in a cross-Nicol configuration, with the side of the cross-sectional piece corresponding to the thickness direction of the optically anisotropic film (see FIG. 5) being parallel to the transmission axis of one of the polarizing plates. Next, the slide glass was rotated using an extinction degree measuring device (manufactured by Otsuka Electronics Co., Ltd., measurement wavelength: 550 nm) to confirm the rotation position at which the light was quenched. At this time, as shown in FIG. 6, the cross-sectional slice was divided into three regions along the side 18E corresponding to the thickness direction of the optically anisotropic film of the cross-sectional slice 18, and the side where the photo-aligned composition layer was arranged was region R1, the air interface side was region R3, and the region between them was region R2. The more uniform the tilt angle of the liquid crystal compound in the thickness direction of the optically anisotropic film, the more uniform the alignment direction of the liquid crystal compound LC in the regions R1 to R3, so that when the slide glass was rotated as described above, the difference in the rotation angle at which the light was quenched in the regions R1 to R3 is small. If the liquid crystal compound is not aligned in any of the regions R1 to R3, that region will not be quenched. The above measurements were carried out and evaluated according to the following criteria. AA: The rotation angle at which the light is extinct in each of the three divided regions is within the range of ±2°. A: The rotation angle at which light is extinct in each of the three divided regions is in the range of more than ±2° and is in the range of ±5° or less. B: The extinction rotation angle of each of the three divided regions is wider than ±5°. C: No quenching in at least one of the three divided regions.
[0080] The results are summarized in Table 1. In Table 1, "Number of benzene rings" indicates the type of liquid crystal composition used, and the number in parentheses indicates the number of benzene rings in the liquid crystal compound used in the liquid crystal composition. In Examples 1 to 5, the irradiation direction of the ultraviolet light irradiated onto the photoalignment composition layer and the application direction of the magnetic field were both parallel and at an angle of 45°.
[0081] [Table 1]
[0082] As shown in Table 1, it was confirmed that the manufacturing method of the present invention can obtain the desired effects. It was confirmed from a comparison of Examples 1 to 5 that when the magnetic flux density was 0.4 T or more, the effect was more excellent. [Explanation of symbols]
[0083] 10 Base material 12 Photoalignment composition layer 14 Liquid crystal composition layer 16 Optically anisotropic film 18 Cross section
Claims
1. A method for producing an optically anisotropic film using a liquid crystal composition containing a polymerizable liquid crystal compound having magnetic field responsiveness, comprising the steps of: Step 1 of applying a photoalignment composition onto a substrate to form a photoalignment composition layer; Step 2 of irradiating the surface of the photoalignment composition layer with unpolarized and collimated ultraviolet light from an oblique direction; Step 3: applying the liquid crystal composition onto the photoalignment composition layer irradiated with ultraviolet light to form a liquid crystal composition layer; a step 4 of applying a magnetic field to the liquid crystal composition layer at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state along a magnetic field application direction that forms an angle of 3° or less with the irradiation direction of the ultraviolet light in the step 2; and a step 5 of curing the liquid crystal composition layer in this order.
2. A method for producing an optically anisotropic film using a liquid crystal composition containing a polymerizable liquid crystal compound having magnetic field responsiveness, comprising the steps of: Step 1 of applying a photoalignment composition onto a substrate to form a photoalignment composition layer; Step 2 of irradiating the surface of the photoalignment composition layer with unpolarized and collimated ultraviolet light from an oblique direction; Step 3: applying the liquid crystal composition onto the photoalignment composition layer irradiated with ultraviolet light to form a liquid crystal composition layer; a step 4 of applying a magnetic field to the liquid crystal composition layer at a temperature at which the liquid crystal composition in the liquid crystal composition layer exhibits an aligned state along a magnetic field application direction that forms an angle of 3° or less with the irradiation direction of the ultraviolet light in the step 2; and step 5 of curing the liquid crystal composition layer, A method for producing an optically anisotropic film, comprising: placing a cross-sectional slice of the optically anisotropic film between two polarizing plates arranged in a cross-Nicol configuration; dividing the cross-sectional slice into three regions along an edge corresponding to the thickness direction of the optically anisotropic film; and rotating the cross-sectional slice of the optically anisotropic film, the difference in rotation angle at which light is extinct in the three regions is within a range of ±5° or less.
3. 3. The method for producing an optically anisotropic film according to claim 1, wherein in the step 2, the irradiation direction of the ultraviolet ray is at an angle of 5 to 85° with respect to a normal direction of the surface of the photoalignment composition layer.
4. 4. The method for producing an optically anisotropic film according to claim 1, wherein the polymerizable liquid crystal compound is a rod-like liquid crystal compound having three or more benzene rings.
5. The method for producing an optically anisotropic film according to any one of claims 1 to 4, wherein in the step 4, the magnetic field has a magnetic flux density of 0.2 to 1.0 T.
Citation Information
Patent Citations
Method for manufacturing optically anisotropic polymer molding
JP2003195050A
Manufacturing method for optical anisotropic film with oblique optical axis
JP2003255127A
Method of manufacturing optical element
JP2005173503A
Method for manufacturing optical film
JP2005316175A
Method for manufacturing optically anisotropic polymer thin film
JP2008076790A