Phenothiazine compounds, their preparation and use as antiaging, antioxidant, antiozonant and coloring agents in rubber blends and vehicle tires
Phenothiazine derivatives like 3-(1,3-dimethylbutylamino)phenothiazine address the health and solubility issues of aromatic amines by enhancing solubility and reactivity, improving the anti-aging performance of vehicle tires and industrial rubber articles.
Patent Information
- Application Number
- JP2023519834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-02
- Filing Date
- 2021-09-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-29
AI Technical Summary
Existing anti-aging agents for vehicle tires and industrial rubber articles, such as aromatic amines, pose health risks and exhibit blooming behavior, leading to reduced protective effects due to low solubility and migration, and can cause premature crosslinking or scorching.
The use of phenothiazine derivatives, specifically 3-(1,3-dimethylbutylamino)phenothiazine, which offers improved solubility and stability, enhancing the protective effect against oxidation and ozone deterioration while minimizing health hazards.
The phenothiazine derivatives provide better solubility and reactivity towards free radicals, resulting in improved durability and reduced blooming, thus maintaining effective anti-aging properties in rubber articles.
Smart Images

Figure 0007559232000036 
Figure 0007559232000037 
Figure 0007559232000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound, a rubber mixture comprising said compound, a vehicle tyre comprising said rubber mixture in at least one component, a process for the preparation of said compound and the use of said compound as antiaging agent and / or antioxidant and / or antiozonant and / or pigment. [Background technology]
[0002] Vehicle tires and industrial rubber articles are known to employ polymeric materials, particularly rubber.
[0003] During long-term storage, especially in end use, which is often at high temperatures, natural rubber and synthetic polymers (IR, BR, SBR, ESBR, etc.), as well as natural and synthetic oils, fats, and lubricants, undergo oxidation reactions that adversely affect their original desirable properties. Depending on the type of polymer, the polymer chains become so short that liquefaction or subsequent hardening of the material occurs.
[0004] Antioxidants therefore play a crucial role in the durability of vehicle tires and other industrial rubber articles.
[0005] Known antioxidants are aromatic amines, such as 6-PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine), IPPD (N-isopropyl-N'-phenyl-p-phenylenediamine) or SPPD (N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine).
[0006] These molecules are capable of reacting with oxygen or ozone or with free radicals formed, such as alkyl and alkylperoxy radicals, thereby scavenging them and thereby protecting rubbers and the like from further oxidation reactions.
[0007] However, aromatic amines have the drawback of being suspected carcinogens and therefore harmful to health, in particular because aniline or its derivatives can be liberated.
[0008] Furthermore, the solubility of the antioxidant in the medium to be protected must be taken into account. Antioxidants such as IPPD sometimes have the disadvantage of being poorly soluble in rubber and therefore migrate to the surface where they form a film, which is usually colored. This effect is known as "blooming" and the antioxidants bloom out of the respective rubber. In addition to appearance, this also has the disadvantage that the bloomed antioxidants are removed, for example by rain, resulting in a continuous decrease in the concentration of the antioxidant in the medium to be protected, with the result that the film is reformed by further migration of the molecules. This results in a reduced protection effect compared to the case without blooming and loss of antioxidant.
[0009] In particular, antioxidants that react with and capture ozone are also called "antiozonants." Summary of the Invention [Problem to be solved by the invention]
[0010] The aim of the present invention is to provide compounds which can be used in particular as anti-aging agents for vehicle tyres or other industrial rubber articles, in order to achieve an improved protective effect for these articles based on the prior art. In particular, the blooming behaviour must be improved, while at the same time providing compounds which are less harmful to health compared to the prior art (aromatic amines). [Means for solving the problem]
[0011] This object is achieved by the inventive compound according to claim 1, by an inventive rubber mixture comprising said compound and by an inventive vehicle tyre comprising in at least one component thereof a rubber mixture according to the invention. This object is further achieved by a process for the preparation of said compound and by the use of said compound with antiaging agents and / or antioxidants and / or antiozonants.
[0012] The compounds according to claim 1 can further be used as dyes. [Brief description of the drawings]
[0013] [Figure 1a] The value indicates the associated cleavage mechanism. [Figure 1b] The value indicates the associated cleavage mechanism. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The compound of claim 1 has formula I: [ka] has.
[0015] Thus, the compound of formula I) is 3-(1,3-dimethylbutylamino)phenothiazine.
[0016] The compounds of formula I) are phenothiazine derivatives. Phenothiazines / derivatives thereof are used as medicines, inter alia, for the treatment of, for example, Parkinson's disease (see US 20130315825 A1), and are less harmful to health than aromatic amines such as 6PPD or IPPD.
[0017] However, phenothiazine itself is not easily soluble in polymers such as the rubber of vehicle tires or other industrial rubber articles, resulting in the blooming problem mentioned above.The compounds according to the invention therefore have the advantage of a better protective effect compared to phenothiazine.
[0018] At the same time, the compounds according to the invention of formula I) show improved protective effect, especially compared to known anti-aging agents such as 6PPD, which is believed to be due to their high reactivity towards free radicals, although the invention is not bound by any particular mechanism of action or any particular explanation.
[0019] US Patent No. 3,413,291 discloses phenothiazine derivatives. However, the derivatives disclosed therein are also not easily soluble in rubber, such as N-isopropyl-10H-phenothiazine-3-amine. Therefore, the compound of the present invention of formula I) shows better solubility in polymers such as rubber and thus improved protective effect compared to known phenothiazine derivatives due to the 1,3-dimethylbutyl group.
[0020] Chinese Patent No. 108069874 also discloses anti-aging agents based on phenothiazine derivatives. However, the derivatives disclosed therein, due to the substituents, do not simultaneously contain the moiety R 2 It is a Schiff base with C=NR' (R' is H, not hydrogen). [ka]
[0021] These substances have sp ions near the phenyl-N group as shown in S2). 3 Due to the absence of hybrid α-H atoms (α-hydrogen atoms), it is presumed to be susceptible to hydrolysis and to have a low protective effect. [ka]
[0022] Thus, compared to such Schiff base phenothiazine derivatives such as the compounds of formula S1), the compounds of the present invention of formula I) have the advantage of being more stable, less susceptible to hydrolysis and allowing for better protective effects.
[0023] Chinese Patent No. 106590827 describes formula S3): [ka] This publication discloses phenothiazine derivatives of the formula:
[0024] However, the compounds of formula S3) have the disadvantage that the -S-CH2-NH- moiety is susceptible to hydrolysis, e.g. in rubber mixtures for vehicle tyres, which can lead to the formation / liberation of thiols, which can cause undesirable pre-crosslinking (scorch) of the rubber mixture.
[0025] CN105272892 discloses antioxidants of formula S4) in which phenol derivatives are linked to phenothiazine units through linking groups that are thioacetate and amide. These linking group units are also not advantageous for use in vulcanized rubber mixtures, since thioacetate is a capped mercaptan, which may decompose during vulcanization and combine with, for example, diene-containing rubbers. Furthermore, the amide moiety has no α-H atom, which reduces the effectiveness of the antioxidant as described above with respect to formula S1). [ka]
[0026] Chinese Patent No. 107935867 discloses an anti-aging agent of formula S5) which exhibits a free amine group (-NH2), which increases the risk of premature crosslinking, also called "scorching", in rubber mixtures, for example in vehicle tires or other industrial rubber articles. [ka]
[0027] The inventive compounds of formula I) are particularly suitable as antiaging and / or antiozonant agents in vehicle tyres and / or industrial rubber articles, such as, in particular, air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical or robotic applications or shoe soles or parts thereof, and / or oils and / or lubricants.
[0028] The inventive compounds of formula I) are particularly suitable for the manufacture of rubber articles, in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical or robotic applications or shoe soles or parts thereof.
[0029] To use a compound according to formula I) in the recited article or substance, said compound is used in a composition or is incorporated into said composition.
[0030] In vehicle tyres or other industrial rubber articles, this is especially the rubber mixture.
[0031] The present invention further provides the use of the compounds according to the invention of formula I) in oils and lubricants, in particular fuels or fluids for engines.The compounds according to the invention can therefore be used in engines.
[0032] The present invention further provides the use of the inventive compounds according to formula I) as dyes in fibres and / or polymers and / or paper and / or paints and coatings.
[0033] The invention therefore further provides a rubber mixture as described above.
[0034] The rubber mixtures according to the invention contain a compound of formula I. They may in principle be any rubber mixture in which the novel inventive compound of formula I) provides improved properties, in particular increased durability due to antiaging and / or antiozonation effects.
[0035] The rubber mixtures of the present invention contain at least one rubber.
[0036] It is preferred if the rubber mixtures according to the invention contain from 0.1 to 10 phr of compounds of the formula I), particularly preferably from 0.1 to 5 phr and very particularly preferably from 1 to 5 phr.
[0037] The unit "phr" (parts per hundred parts rubber by weight) used herein is a customary designation of quantities for mix recipes in the rubber industry. The amounts in parts by weight of individual materials are herein based on 100 parts by weight of the total mass of all high molecular weight (Mw>20,000 g / mol) and therefore solid rubber present in the mix.
[0038] In an advantageous embodiment of the invention, the rubber mixture according to the invention contains at least one diene rubber.
[0039] Thus, the rubber mixture may contain a diene rubber or a mixture of two or more different diene rubbers.
[0040] Diene rubbers are rubbers formed by the polymerization or copolymerization of dienes and / or cycloalkenes and thus have C=C double bonds either in the backbone or in side groups.
[0041] The diene rubber is preferably natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, molecular weight M wis selected from the group consisting of liquid rubber having a molecular weight greater than 20,000 g / mol, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile butadiene rubber, and hydrogenated styrene-butadiene rubber.
[0042] Nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber, and / or ethylene-propylene-diene rubber are used in particular for the manufacture of industrial rubber articles such as belts, drive belts, and hoses, and / or shoe soles. It is preferable to employ the mixture compositions known to those skilled in the art for these rubbers (specifically referred to as fillers, plasticizers, vulcanization systems, and additives).
[0043] The natural and / or synthetic polyisoprene in all embodiments can be either cis-1,4-polyisoprene or 3,4-polyisoprene. However, it is preferred to use cis-1,4-polyisoprene with a cis-1,4 ratio of more than 90% by weight. Such polyisoprene can be obtained, firstly, by stereospecific polymerization in solution using Ziegler-Natta catalysts or by using finely dispersed lithium alkyls. Secondly, natural rubber (NR) is one of such cis-1,4-polyisoprenes, and the cis-1,4 content in natural rubber is higher than 99% by weight.
[0044] Additionally, mixtures of one or more natural polyisoprenes with one or more synthetic polyisoprenes are contemplated.
[0045] In the context of the present invention, the term "natural rubber" should be understood to mean naturally occurring rubber that can be obtained from Hevea brasiliensis and from "non-Hevea" sources, such as guayule shrub and dandelions, e.g. TKS (Taraxacum kok-saghyz; Russian dandelion).
[0046] If the rubber mixture of the present invention contains butadiene rubber (i.e. BR, polybutadiene), this may be of any type known to those skilled in the art. These include the so-called high cis and low cis types, where polybutadienes with a cis content of 90% or more by weight are called high cis types and polybutadienes with a cis content of less than 90% by weight are called low cis types. An example of a low cis polybutadiene is Li-BR (lithium catalyzed butadiene rubber) with a cis content of 20% to 50% by weight. Particularly good properties and low hysteresis of the rubber mixture are achieved with high cis BR.
[0047] The polybutadienes employed may be end-group modified and / or functionalized along the polymer chain using modifications and functionalizations selected from modifications with hydroxyl groups, and / or ethoxy groups, and / or epoxy groups, and / or siloxane groups, and / or amino groups, and / or aminosiloxanes, and / or carboxyl groups, and / or phthalocyanine groups, and / or silane-sulfide groups. However, other modifications known to those skilled in the art, also known as functionalizing agents, are suitable. Metal atoms may be components of such functionalizations.
[0048] If at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture, it may be either a solution-polymerized styrene-butadiene rubber (SSBR) or an emulsion-polymerized styrene-butadiene rubber (ESBR), and mixtures of at least one SSBR and at least one ESBR may also be used. The terms "styrene-butadiene rubber" and "styrene-butadiene copolymer" are used synonymously in the context of the present invention.
[0049] The styrene-butadiene copolymers used may be end-group modified and / or functionalized along the polymer chain using the modifications and functionalizations cited above for polybutadiene.
[0050] The at least one diene rubber is preferably selected from the group consisting of natural polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR), and halobutyl rubber.
[0051] In a particularly preferred embodiment of the present invention, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), and emulsion polymerized styrene-butadiene rubber (ESBR).
[0052] In a particularly advantageous embodiment of the invention, the rubber mixture comprises at least one natural polyisoprene (NR), preferably in an amount of 5 to 55 phr, in one particularly advantageous embodiment of the invention from 5 to 25 phr, very preferably from 5 to 20 phr. Such rubber mixtures exhibit good processability and recovery stability, as well as optimized tear properties and optimal rolling resistance properties.
[0053] In a particularly advantageous embodiment of the invention, the rubber mixture comprises at least one polybutadiene (BR, butadiene rubber), preferably in an amount of 10 to 80 phr, particularly preferably 10 to 50 phr and in a particularly advantageous embodiment of the invention 15 to 40 phr, whereby particularly good tear and wear properties as well as optimal braking properties of the rubber mixture according to the invention are achieved.
[0054] In a particularly advantageous embodiment of the invention, the rubber mixture comprises at least one solution polymerized styrene-butadiene rubber (SSBR), preferably in an amount of 10 to 80 phr, particularly preferably 30 to 80 phr, and in one particularly advantageous embodiment of the invention, 50 to 70 phr. This achieves particularly good rolling resistance properties of the rubber mixture according to the invention. In a particularly advantageous embodiment of the invention, the SSBR is employed in combination with at least one additional rubber in order to achieve an optimal and balanced profile of properties.
[0055] It is preferred that the rubber mixture comprises at least one filler, preferably in an amount of 30 to 500 phr, particularly preferably 50 to 400 phr, next more preferably 80 to 300 phr.
[0056] In an advantageous embodiment of the invention, the filler is a reinforcing filler, preferably selected from the group consisting of carbon black and silica.
[0057] In a particularly advantageous embodiment of the invention, the rubber mixture comprises at least one silica as filler, preferably in an amount of 30 to 500 phr, particularly preferably 50 to 400 phr, next more preferably 80 to 300 phr.
[0058] In these amounts, silica is typically present as the sole or predominant filler (greater than 50% by weight based on total filler).
[0059] In a further advantageous embodiment of the invention, the rubber mixture comprises at least one silica as additional filler, preferably in an amount of 5 to 100 phr, particularly preferably 5 to 80 phr, next more preferably 10 to 60 phr.
[0060] In these amounts, the silica is particularly present as an additional filler in addition to another major filler such as carbon black.
[0061] The silica may be any type of silica known to those skilled in the art that is suitable as a filler for tire rubber compounds. 2 / g, preferably 35 to 350m 2 / g, more preferably 85 to 320 m 2 / g, most preferably 120 to 235 m 2 / g nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) and 30-400 m 2 / g, preferably 30 to 330m 2 / g, more preferably 80 to 300m 2 / g, most preferably 115 to 200m 2 It is particularly preferred to use finely divided precipitated silicas having a CTAB surface area (according to ASTM D 3765) of 10 ...
[0062] If, in the rubber mixture according to the invention, at least two different silicas are present which differ, for example, in terms of their BET surface area, the stated amount figures refer to the total amount of all silicas present.
[0063] The terms "silicic acid" and "silica" are used synonymously in the context of the present invention.
[0064] The rubber mixture may additionally comprise further fillers, such as in particular carbon black, in particular technical carbon black or pyrolytic carbon black, or further reinforcing or non-reinforcing fillers.
[0065] In the context of the present invention, further (non-reinforcing) fillers include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gels and also fibres (eg aramid fibres, glass fibres, carbon fibres, cellulose fibres).
[0066] Further, optionally reinforcing fillers include, for example, carbon nanotubes (CNTs), including discrete CNTs, hollow carbon fibers (HCFs) and modified CNTs containing one or more functional groups, such as hydroxy, carboxy and carbonyl groups, graphite and graphene, and what are known as "carbon-silica dual phase fillers."
[0067] In the context of the present invention, zinc oxide is not included in the filler.
[0068] In a particularly advantageous embodiment of the invention, the rubber mixture according to the invention comprises from 0.1 to 60 phr, preferably from 3 to 40 phr, particularly preferably from 5 to 30 phr and very particularly preferably from 5 to 15 phr of at least one carbon black. In these amounts, the carbon black is especially present as a further filler in addition to the main fillers, such as silica.
[0069] In a further advantageous embodiment of the invention, the rubber mixture according to the invention comprises from 30 to 300 phr, preferably from 30 to 200 phr, particularly preferably from 40 to 100 phr, of at least one carbon black. In these amounts, the carbon black is present as the only or main filler, and therefore optionally in combination with small amounts of silica as mentioned above.
[0070] Suitable carbon blacks include any type of carbon black known to those skilled in the art.
[0071] In one embodiment, the carbon black has an iodine number (also called iodine adsorption) according to ASTM D 1510 of 30 to 250 g / kg, preferably 30 to 180 g / kg, particularly preferably 40 to 180 g / kg, very preferably 80 to 150 g / kg, and a DBP number according to ASTM D 2414 of 30 to 200 mL / 100 g, preferably 70 to 200 mL / 100 g, particularly preferably 90 to 200 mL / 100 g.
[0072] The DBP number according to ASTM D 2414 defines the specific absorption volume of carbon black or light colored fillers with dibutyl phthalate.
[0073] The use of such types of carbon black in rubber mixtures, especially in vehicle tires, allows for the best compromise between wear resistance and heat storage, with a consequent positive effect on the ecologically relevant rolling resistance. In this case, it is preferable to use only one type of carbon black in each rubber mixture, although it is also possible to incorporate various types of carbon black into the rubber mixtures.
[0074] In a particularly advantageous embodiment of the invention, the rubber mixture contains from 5 to 60 phr, particularly preferably from 5 to 40 phr, of at least one carbon black and from 50 to 300 phr, preferably from 80 to 200 phr, of at least one silica.
[0075] The rubber mixture may further contain conventional additives in conventional parts by weight, which are preferably added in at least one primary mixing stage during the preparation of said mixture. These additives include: a) antioxidants known in the prior art, for example diamines such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD) or dihydroquinolines such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators, such as zinc oxide and fatty acids (e.g. stearic acid) and / or other activators (such as zinc complexes, e.g. zinc ethylhexanoate); c) activators and / or agents for binding fillers, in particular carbon black or silica, such as S-(3-aminopropyl)thiosulfate and / or its metal salts (carbon black binding) and silane coupling agents (silica binding); d) ozone degrading wax, e) resins, especially tackifying resins for internal tire components; f) mastication aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD), and g) processing aids, such as in particular fatty acid esters and metal soaps, such as zinc soaps and / or calcium soaps; h) plasticizers, for example in particular aromatic, naphthenic or paraffinic mineral oil plasticizers, for example MES (Mild Extraction Solvates), preferably having a content of polycyclic aromatic compounds of less than 3% by weight according to method IP 346, or RAE (Residual Aromatic Extract), or TDAE (Processed Distillate Aromatic Extract), or Rubber to Liquid (RTL) oils or Biomass to Liquid (BTL) oils, or triglycerides, for example rapeseed oil or factice, or hydrocarbon resins or liquid polymers with an average molecular weight (determined by GPC = Gel Permeation Chromatography in accordance with BS ISO 11344:2004) of 500 to 20,000 g / mol.
[0076] If a mineral oil is used, it is preferably selected from the group consisting of DAE (Distillate Aromatic Extract), and / or RAE (Residual Aromatic Extract), and / or TDAE (Treated Distillate Aromatic Extract), and / or MES (Mild Extraction Solvates), and / or naphthenic oils.
[0077] In a particularly advantageous embodiment, the rubber mixture according to the invention does not contain, in addition to the inventive compound of formula I), further antiaging agents from the group of the p-phenylenediamines (see list a) above). In a particularly preferred embodiment, the rubber mixture according to the invention comprises 0 to 0.1 phr, in particular 0 phr, of a further antiaging agent based on diamines, particularly preferably selected from the group consisting of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD).
[0078] The presence according to the invention of the abovementioned diamines and compounds of formula I in very small amounts, preferably 0 to 0 phr, particularly preferably 0 phr, makes it possible to achieve an improved protective effect. The inventive compounds of formula I) replace the listed diamines known in the prior art.
[0079] In a further advantageous embodiment of the present invention, at least one further representative of the listed diamine antioxidants is present, so that the compounds according to the invention only partially replace the diamines known in the prior art, which also benefit from the present invention, but not to an optimal extent.
[0080] In an advantageous embodiment, in addition to the inventive compound of formula I), an antioxidant based on dihydroquinoline, such as TMQ, is present in the rubber mixture. The amount of dihydroquinoline, such as TMQ, present is preferably from 0.1 to 3, in particular from 0.5 to 1.5 phr.
[0081] In a further advantageous embodiment, the rubber mixture according to the invention does not comprise further anti-aging agents, i.e. it comprises 0 phr of further anti-aging agents other than the inventive compound of formula I).
[0082] The silane coupling agent may be of any type known to those skilled in the art.
[0083] Furthermore, one or more different silane coupling agents may be used in combination with one another, and the rubber mixture may therefore contain a mixture of different silanes.
[0084] The silane coupling agent reacts with the surface silanol groups or other polar groups of the silica either during mixing of the rubber / rubber mixture (in situ) or in a pretreatment (pre-modification) situation even before addition of the filler to the rubber.
[0085] Coupling agents known from the prior art are bifunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as leaving group on the silicon atom and, optionally, as another functional group, a group which, after cleavage, can enter into a chemical reaction with the double bond of the polymer. The latter group can, for example, include the following chemical groups: -SCN, -SH, -NH2 or -S x -(x=2~8).
[0086] Thus, usable silane coupling agents may be, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane, or 3,3'-bis(triethoxysilylpropyl) polysulfides having 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfides (TESPD), or mixtures of sulfides having 1 to 8 sulfur atoms with different sulfide contents. TESPT may also be added, for example, as a mixture with carbon black (trade name X50S® from Evonik).
[0087] Blocked mercaptosilanes, such as known from WO 99 / 09036, can also be used as silane coupling agents.It is also possible to use silanes such as those described in WO 2008 / 083241A1, WO 2008 / 083242A1, WO 2008 / 083243A1 and WO 2008 / 083244A1.It is also possible to use silanes such as those sold under the name NXT by Momentive, USA in many variations, or those sold under the name VP Si 363® by Evonik Industries.
[0088] The total proportion of further additives is preferably between 3 and 150 phr, more preferably between 3 and 100 phr, most preferably between 5 and 80 phr.
[0089] Zinc oxide (ZnO) may be included in the overall proportion of further additives in the amounts mentioned above.
[0090] This can be any type of zinc oxide known to those skilled in the art, for example ZnO granules or powder. Conventionally used zinc oxides usually have a BET specific surface area of 10 m 2 / g. However, the range is 10 to 100 m 2 It is also possible to use zinc oxide having a BET surface area of 100 nm to 100 nm / g, for example the so-called "nano zinc oxide".
[0091] The rubber mixtures according to the invention are preferably used in vulcanized form, in particular in vehicle tyres or other vulcanized industrial rubber articles.
[0092] The vulcanization of the rubber mixtures of the invention is preferably carried out in the presence of sulfur and / or sulfur donors using vulcanization accelerators, some of which can simultaneously act as sulfur donors, selected from the group consisting of thiazole accelerators, and / or mercapto accelerators, and / or sulfenamide accelerators, and / or thiocarbamate accelerators, and / or thiuram accelerators, and / or thiophosphate accelerators, and / or thiourea accelerators, and / or xanthate accelerators, and / or guanidine accelerators.
[0093] It is preferred to use a sulfenamide based accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazole sulfenamide (CBS), and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS), and / or benzothiazyl-2-sulfenomorpholide (MBS), and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS), or a guanidine accelerator such as diphenylguanidine (DPG).
[0094] The sulfur donor substance used may be any sulfur donor substance known to those skilled in the art. If the rubber mixture contains a sulfur donor substance, the latter is preferably, for example, a thiuram disulfide, such as tetrabenzylthiuram disulfide (TBzTD), and / or tetramethylthiuram disulfide (TMTD), and / or tetraethylthiuram disulfide (TETD), and / or a thiuram tetrasulfide, such as dipentamethylenethiuram tetrasulfide (DPTT), and / or a dithiophosphate, such as DipDis (bis(diisopropyl)thiophosphoryl disulfide), and / or bis(O,O-2-ethylhexylthiophosphoryl) polysulfide (for example Rhenocure SDT 50®, Rheinchemie GmbH), and / or zinc dichloryl dithiophosphate (for example Rhenocure ZDT / S®, Rheinchemie GmbH). GmbH), and / or zinc alkyldithiophosphates, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane, and / or diaryl polysulfides, and / or dialkyl polysulfides.
[0095] Further network-forming systems, such as those available under the trade names Vulkuren®, Duralink® or Perkalink®, or as described in WO 2010 / 049216 A2, can also be used in the rubber mixtures, which contain a vulcanizing agent crosslinking with a functionality greater than 4 and at least one vulcanization accelerator.
[0096] It is particularly preferred to use TBBS, and / or CBS, and / or diphenylguanidine (DPG) as accelerators.
[0097] Vulcanization retarders may also be present in the rubber mixture.
[0098] The terms "vulcanization" and "crosslinking" are used synonymously in the context of this invention.
[0099] In a preferred development of the invention, the vulcanization accelerators are added in the final mixing stage during the preparation of the sulfur-crosslinkable rubber mixture.
[0100] The sulfur-crosslinkable rubber mixtures of the present invention are prepared by processes that are conventional in the rubber industry, in which a base mixture is first prepared, containing all the constituents except the vulcanization system (sulfur and substances that affect the vulcanization), in one or more mixing stages. The finished mixture is prepared by adding the vulcanization system in the final mixing stage. The finished mixture is further processed, for example, by extrusion operations or calendering, to give it a suitable shape.
[0101] This is followed by further processing by sulfur vulcanization, where the sulfur crosslinking occurs due to the vulcanization system added in connection with the present invention.
[0102] The above-mentioned rubber mixtures according to the invention are particularly suitable for use in vehicle tyres, especially pneumatic vehicle tyres.
[0103] For use in vehicle tires, the mixture as a finished pre-vulcanized mixture is preferably formed into a tread and applied in known manner during the manufacture of uncured vehicle tires.
[0104] The preparation of the rubber mixtures of the invention for use as sidewall or other body mixtures in vehicle tires is accomplished as already described. The difference is in the shaping after the extrusion operation / calendering of the mixture. The shaped articles thus obtained of the still unvulcanized rubber mixtures for one or more different body mixtures then serve for the construction of uncured tires.
[0105] "Body mix" herein refers to the rubber mix for the inner components of the tire, such as essentially the squeegee, innerliner, core profile, belt, shoulder, belt profile, carcass, bead reinforcement, bead profile, flange profile, bandage, etc. The still unvulcanized green tire is then vulcanized.
[0106] For the use of the rubber mixture of the invention in drive belts and other belts, especially conveyor belts, the extruded, still unvulcanized mixture is brought into a suitable shape and is often simultaneously or subsequently provided with reinforcing members, such as synthetic fibers or steel cords, which usually gives a multi-ply construction consisting of one and / or several plies of the rubber mixture, one and / or several plies of the same and / or different reinforcing members and one and / or several plies of the same and / or another rubber mixture.
[0107] The present invention further provides a vehicle tyre comprising a rubber mixture according to the invention, which comprises in at least one component a compound according to the invention.
[0108] A vulcanized vehicle tire contains, in at least one component, a vulcanizate of at least one rubber mixture according to the invention. The skilled person is aware that most substances, such as rubbers present, are present in a chemically altered form already after mixing or only after vulcanization.
[0109] In the context of the present invention, "vehicle tyres" should be understood to mean pneumatic vehicle tyres and solid rubber tyres, including tyres for industrial and construction site vehicles, trucks, passenger cars and two-wheeler tyres.
[0110] The vehicle tyre according to the invention preferably comprises the rubber mixture according to the invention in at least one external component, which is preferably the tread, the sidewall and / or the flange profile.
[0111] The vehicle tyres according to the invention may therefore comprise the rubber mixtures according to the invention comprising the inventive compounds of formula I), optionally in two or more components of adapted composition.
[0112] The present invention further comprises the process steps: a) Substance of formula A) [ka] preparing a b) providing methyl isobutyl ketone (MIBK) and hydrogen (H2); c) reacting the material from step a) with the material from step b), preferably in the presence of a hydrogenation catalyst, to obtain a material of formula I) [ka] obtaining the above compound; The present invention provides a method for preparing a compound of formula I, comprising at least
[0113] The present invention further comprises the process steps: a1) Substance of formula A) [ka] preparing a b1) providing a reducing agent, in particular tin(II) chloride dihydrate; c1) reacting the material from step a1) with the material from step b1) to obtain a material of formula C1) [ka] obtaining the above compound; d1) providing methyl isobutyl ketone (MIBK) and hydrogen (H2); e1) reacting the product of formula C1) with a product from step d1), preferably in the presence of a hydrogenation catalyst, to give a product of formula I). [ka] obtaining the above compound; A further method for preparing a compound of formula I) is provided, comprising at least
[0114] The material methyl isobutyl ketone (MIBK) is commercially available.
[0115] The reducing agent may be any reducing agent known to those skilled in the art and suitable for reducing nitro groups (NO2) to amino groups (-NH2). Tin(II) chloride dihydrate is particularly suitable. It is commercially available.
[0116] The process of steps a) to c) is preferable since it requires fewer process steps than the process of steps a1) to e1).
[0117] The process steps in which reaction with hydrogen takes place are preferably carried out using a suitable catalyst, which in the context of the present invention is referred to as a "hydrogenation catalyst".
[0118] The hydrogenation catalyst of the process (step c) / e1)) is preferably a noble metal catalyst, in particular palladium (Pd) or platinum (Pt). The noble metal is preferably used on carbon (C), such as palladium on carbon (Pd / C) or platinum on carbon (Pt / C).
[0119] Other known catalysts such as Raney nickel or copper chromite may also be employed.
[0120] It is preferred if Pt / C is used in step c).
[0121] It is preferred if Pd / C is used in step e1).
[0122] The hydrogen pressure in each process step in which hydrogen is used is preferably between 1 and 50 bar, particularly preferably between 10 and 45 bar. According to an advantageous embodiment of the invention, pressures between 20 and 40 bar are preferred.
[0123] The hydrogenation reaction in step c) / e1) is preferably carried out in an autoclave, in particular a stainless steel autoclave.
[0124] The temperature in the process steps c) and e1) is preferably between room temperature (RT, in particular 20°C) and 150°C, preferably up to 130°C.
[0125] The present invention further comprises the process steps: a2) A substance of formula A2): [ka] preparing a b2) providing elemental sulfur and o-dichlorobenzene; c2) reacting the material of step a2) with the material of step b2) to obtain a material of formula I) [ka] obtaining the above compound; A further method for preparing a compound of formula I) is provided, comprising at least
[0126] In the following the invention will be elucidated in more detail with reference to examples. EXAMPLES
[0127] The components of formula I) were prepared as follows: X1): Synthesis of the compound of the invention of formula I) (3-(1,3-dimethylbutylamino)phenothiazine) according to process steps a) to c): [ka] 0.50 g (2.05 mmol, 1 equiv.) of 3-nitrophenothiazine, 0.18 g of platinum on carbon (5%) (0.4 g for 4.67 mmol of support) and 20.0 mL of methyl isobutyl ketone were weighed into a stainless steel autoclave with a Teflon-lined liner. The autoclave was then pressurized to 40 bar with hydrogen and stirred at 120° C. for 10 h. After completion of the reaction, the excess hydrogen was bled off and the suspension was filtered through diatomaceous earth (Celite®) and washed with ethanol. The filtrate was concentrated to dryness and vacuum dried. Grey to purple solid; yield 0.57 g (93% of theory). 1H-NMR(500MHz,DMSO-d6)δ=8.09(s,1H),6.94(td,J=7.6,1.5Hz,1H),6.88(dd,J=7.6,1.4Hz,1H ),6.69-6.63(m,2H),6.51(d,J=8.4Hz,1H),6.27(dd,J=8.5,2.5Hz,1H),6.21(d,J=2.5Hz,1H),4 .82(d,J=8.9Hz,1H),3.30(dt,J=8.6,6.5Hz,1H),1.70(dp,J=13.5,6.7Hz,1H),1.38(dt,J=13. 9,7.1Hz,1H),1.16(dt,J=13.5,6.8Hz,1H),1.02(d,J=6.1Hz,3H),0.87(dd,J=19.4,6.6Hz,6H). 13 C-NMR(126MHz,DMSO-d6)δ=144.5,143.9,131.8,127.7,126.6,121.0,117 .6,116.5,115.8,114.4,112.1,110.7,46.5,46.4,25.0,23.2,23.0,21.2. ESI-MS (electrospray ionization mass spectrometry) [M+H] + =299.
[0128] In an additional experiment X2), the reaction was carried out as described above, with the difference that the mixture was stirred at 40° C. for 3 hours while the autoclave was also pressurized to 40 bar with hydrogen.
[0129] Similar yields are obtained as shown in Table 1 below.
[0130] [Table 1]
[0131] The starting material 3-nitrophenothiazine of formula A) according to the above description of the process was prepared according to the disclosure of US Patent Application Publication No. 20130315825A1.
[0132] Alternatively, 3-nitrophenothiazine can be prepared by a one-step copper (Cu) catalyzed synthesis as disclosed in WO 2017011531 A2 (p217). In addition, 3-nitrophenothiazine can be obtained by a non-catalyzed reaction as disclosed in S. Wu, W. Hu, S. Zhang, RSC Advances, 2016, 6(29), 24257-24260. In addition, 3-nitrophenothiazine can be obtained from phenothiazine by reaction with sodium nitrite as disclosed in WO 2007110627 A2.
[0133] Alternatively, the substances of formula I) were obtained starting from 3-nitrophenothiazine in a two-step reaction according to process steps a1) to e1).
[0134] Synthesis of 3-aminophenothiazine: [ka] Under protective gas, 22 g (90.0 mmol, 1.0 equiv.) of 3-nitrophenothiazine were weighed out, dissolved in 800 mL of ethanol, mixed with 102 g (534 mmol, 5.0 equiv.) of tin(II) chloride dihydrate and stirred at boiling heat for 4 days. After the reaction was brought to room temperature (RT), one third of the solvent was distilled off and the remainder was poured onto ice. The pH of the mixture was subsequently adjusted to pH=7 using aqueous potassium hydroxide solution and extracted three times with ethyl acetate. The organic phase was washed with saturated NaCl solution and subsequently dried over Na2SO4. A brown solid was obtained; yield 18.9 g (98% of theory). 1H-NMR(500MHz,DMSO-d6)δ=8.08(s,1H),6.94(td,J=7.7,1.5Hz,1H),6.88(dd,J=7.7 ,1.5Hz,1H),6.71-6.60(m,2H),6.46(d,J=8.3Hz,1H),6.32-6.22(m,H),4.64(s,2H). ESI-MS [M+H] + =215.
[0135] Synthesis of 3-(1,3-dimethylbutylamino)phenothiazine: [ka] 5.00 g (23.3 mmol, 1 equiv.) of 3-aminophenothiazine, 2.00 g of palladium on carbon (5%) (0.4 g for 4.67 mmol of support), and 50.0 mL of methyl isobutyl ketone were weighed into a stainless steel autoclave with a Teflon-lined liner. The autoclave was then pressurized to 40 bar with hydrogen and stirred at 120° C. for 10 h. After completion of the reaction, the excess hydrogen was flashed off and the suspension was filtered through diatomaceous earth (Celite®) and washed with ethanol. The filtrate was concentrated to dryness and vacuum dried. Grey to purple solid; yield 6.61 g (95% of theory). 1 H-NMR(500MHz,DMSO-d6)δ=8.09(s,1H),6.94(td,J=7.6,1.5Hz,1H),6.88(dd,J=7.6,1.4Hz,1H ),6.69-6.63(m,2H),6.51(d,J=8.4Hz,1H),6.27(dd,J=8.5,2.5Hz,1H),6.21(d,J=2.5Hz,1H),4 .82(d,J=8.9Hz,1H),3.30(dt,J=8.6,6.5Hz,1H),1.70(dp,J=13.5,6.7Hz,1H),1.38(dt,J=13. 9,7.1Hz,1H),1.16(dt,J=13.5,6.8Hz,1H),1.02(d,J=6.1Hz,3H),0.87(dd,J=19.4,6.6Hz,6H). 13 C NMR(126MHz,DMSO-d6)δ 144.5,143.9,131.8,127.7,126.6,121.0,117.6,116.5,115.8,114.4,112.1,110.7,46.5,46.4,25.0,23.2,23.0,21.2. ESI-MS [M+H] + =299.
[0136] Alternatively, the substance of formula I) was obtained in a one-step reaction according to process steps a2) to c2).
[0137] Synthesis of 3-(1,3-dimethylbutylamino)-phenothiazine: [ka] Under protective gas, 10 g (37.3 mmol, 1 equiv.) of 6-PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) were dissolved in 80 mL of degassed o-dichlorobenzene and mixed with 2.9 g (89 mmol, 2.4 equiv. based on elemental "S") of sulfur and 0.95 g (3.73 mmol, 0.1 equiv.) of iodine (I2). The mixture was heated to reflux (180 °C) for 4 h. The formed hydrogen sulfide was passed through a 5% NaOH solution. After cooling to room temperature (RT), the mixture was mixed with dichloromethane (DCM) and saturated Na2S2O3 solution. The resulting black solid was removed by filtration and the organic phase was separated from the aqueous phase. The organic phase was washed with saturated NaCl solution, dried over Na2SO4 and concentrated to dryness. The black solid was analyzed by LC-MS (liquid chromatography-mass spectrometry) combined with UV-VIS spectroscopy (ultraviolet and visible spectroscopy). It contained 39% (E)-N-(4-methylpentan-2-yl)-3H-phenothiazine-3-imine (the small molecule to the right of the reaction arrow) and 24% undefined material as by-products. The remaining 37% consisted of starting material and the compound of the invention of formula I).
[0138] The compounds of the invention of formula I) show increased reactivity compared to 6PPD. This is evident, for example, from the calculation of the bond dissociation energy (BDE) as well as the free activation enthalpy Δ R G ≠ and free standard reaction enthalpy Δ R The values are reported in Table 2. Figures 1a and 1b show the cleavage mechanism to which these values relate.
[0139] [Table 2]
[0140] As is evident from Table 2, the compounds of formula I) of the present invention exhibit lower bond dissociation energies and lower free enthalpies.
[0141] Thus, with the compounds of formula I) it is possible to achieve improved protective effects in the applications listed.
[0142] For use in rubber mixtures for vehicle tyres, the compounds of formula I) according to the invention are added in a manner known to those skilled in the art during one of the mixing stages in the preparation of the rubber mixture, instead of the antiaging agents known from the prior art, such as, for example, 6PPD, 7PPD or IPPD. While this application is directed to the invention set forth in the claims, the disclosure of this application also includes: 1. Formula I below: [ka] Compound. 2. Rubber mixtures containing a compound of formula I) as defined in 1. above. 3. The rubber mixture according to claim 2, further comprising at least one diene rubber. 4. The rubber mixture according to 3., characterized in that it contains at least one diene rubber selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR), and halobutyl rubber. 5. A vehicle tire comprising in at least one component thereof the rubber mixture according to any one of claims 2 to 4. 6. A vehicle tire according to claim 5, in which at least one external component comprises at least one rubber mixture according to any one of claims 2 to 4, said external component being preferably a tread, a sidewall and / or a flange profile. 7. The process steps are as follows: a) Substance of formula A) [ka] preparing a b) Methyl isobutyl ketone (MIBK) and hydrogen (H 2 ) preparing a solution; c) reacting said material from step a) with said material from step b) to obtain a material of formula I) [ka] obtaining the above compound; A method for producing the compound of formula I) described in 1. above, comprising at least the steps of: 8. The following process steps: a1) Substance of formula A) [ka] preparing a b1) providing a reducing agent, in particular tin(II) chloride dihydrate; c1) reacting said material from step a1) with said material from step b1) to obtain a material of formula C1)
change
change
change
change
Claims
1. The following formula I): 【Chemistry 1】 Compound.
2. 2. Rubber mixtures comprising a compound of formula I) according to claim 1.
3. 3. The rubber mixture according to claim 2, characterized in that it contains at least one diene rubber.
4. 4. The rubber mixture according to claim 3, characterized in that it contains at least one diene rubber selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR), and halobutyl rubber.
5. A vehicle tyre comprising in at least one component a rubber mixture according to any one of claims 2 to 4.
6. Vehicle tyre according to claim 5, comprising in at least one external component at least one rubber mixture according to any one of claims 2 to 4.
7. The process steps are as follows: a) a substance of formula A) 【Chemistry 2】 preparing a b) Methyl isobutyl ketone (MIBK) and hydrogen (H 2 ) ; c) reacting said material from step a) with said material from step b) to obtain a material of formula I) 【Chemistry 3】 obtaining A method for preparing a compound of formula I) according to claim 1, comprising at least
8. The process steps are as follows: a1) Substance of formula A) 【Chemistry 4】 preparing a b1) providing a reducing agent; c1) reacting said material from step a1) with said material from step b1) to obtain a material of formula C1) 【Chemistry 5】 obtaining d1) Methyl isobutyl ketone (MIBK) and hydrogen (H 2 ) providing a e1) reacting said material of formula C1) with said material from step d1) to give a material of formula I) 【Chemistry 6】 obtaining A method for preparing a compound of formula I) according to claim 1, comprising at least
9. The process steps are as follows: a2) A substance of formula A2): 【Chemistry 7】 preparing a b2) providing elemental sulfur and o-dichlorobenzene (orthodichlorobenzene); c2) reacting said material from step a2) with said material from step b2) to obtain a material of formula I). 【Chemistry 8】 obtaining A method for preparing a compound of formula I) according to claim 1, comprising at least 10. Use of a compound of formula I) as claimed in claim 1 as an anti-aging agent and / or anti-ozonant in vehicle tyres and / or industrial rubber articles and / or oils and / or lubricants.
11. Use of a compound of formula I) as defined in claim 1 as an anti-aging and / or anti-ozonant in a fuel or fluid for an engine.
Citation Information
Patent Citations
Cardanol-based antioxidant as well as preparation method and application thereof
CN107935867A
Novel Schiff base type amine antioxidant as well as preparation method and application thereof
CN108069874A
Production of diaminodiphenylamine derivative useful as degradation preventing agent
JP1998168038A
Method for preparation of 4,4'-dinitrodiphenylamine and 4,4'-bis(alkylamino)diphenylamine by using 4-nitroaniline
US20120157714A1
Hydrocarbylamino phenoxazines and phenazines
US3413291A