Polymerizable liquid crystal composition

A dual anisotropic LCP composition addresses wavelength-dependent polarization issues in optical films by using two distinct LCP compounds with specific ring structures and additives, achieving uniform polarization conversion and reduced coloration.

JP7564192B2Active Publication Date: 2024-10-08ROLIC TECHNOLOGIES AG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022513197
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-28
Filing Date
2020-08-24
Publication Date
2024-10-08
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Existing optical films using single anisotropic liquid crystal (LCP) compounds suffer from wavelength-dependent polarization conversion, leading to colored light and non-uniform optical performance due to tilt domains and disclinations, necessitating improved compositions with broader wavelength dispersion and higher uniformity.

Method used

A composition comprising at least two different anisotropic LCP compounds, each with specific ring structures and additives, is formulated to enhance polarization conversion and reduce tilt domains, using crosslinkable LCPs applied on substrates with alignment layers and photoaligning techniques to achieve uniform alignment.

Benefits of technology

The dual LCP composition achieves improved uniform polarization conversion across a wide wavelength range, reducing coloration and enhancing optical film performance by minimizing tilt domains and disclinations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564192000001
    Figure 0007564192000001
  • Figure 0007564192000002
    Figure 0007564192000002
  • Figure 0007564192000003
    Figure 0007564192000003
Patent Text Reader

Abstract

The present invention relates to novel compositions comprising at least two anisotropic compounds of formula (I), as well as liquid crystal networks, films and electro-optical devices comprising said compositions. TIFF2022545818000014.tif65169
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] 2. Background of the Invention The present invention relates to a novel composition comprising at least two different polymerizable anisotropic liquid crystal (LCP) compounds, a formulation comprising such LCP compounds, and an optical film comprising such an LCP composition. The optical film comprising the composition according to the present invention shows an inverse phase difference pattern of polarized light over a wide wavelength range. Finally, the present invention relates to an optically anisotropic article comprising such a composition or comprising an optical film comprising such a composition, such as, for example, a flat panel display, a TV, a smartphone, a tablet.

[0002] Optical films (LCP films) prepared from curable LCP compounds are well known to those skilled in the art and are used in the fabrication of optical devices. An example of an optical film is a retardation film or polarizer. A retardation film is a type of optical element that changes the polarization state of light passing through it. When light passes through a retardation film, the polarization direction of the light changes due to the birefringence and thickness of the film. A quarter-wave retarder converts linearly polarized light into circularly polarized light, and a half-wave retarder converts the vibration plane of linearly polarized light by 90°. Such retardation films can achieve the conversion of a specific monochromatic light so that a λ / 4 or λ / 2 retardation occurs. However, known retardation films have the disadvantage that the polarized light passing through them is converted into colored polarized light. In addition, polarized white light produces a polarization state distribution corresponding to each wavelength. Therefore, it is impossible to achieve a precise λ / 4 or λ / 2 retardation over the entire wavelength range. To improve such disadvantages, it is necessary to develop a retarder film with a higher wavelength dispersion at longer wavelengths than at shorter wavelengths. Another challenge in preparing retardation films, also known as retarders, is preparing high performance films with small amounts of material.

[0003] Therefore, there is a need for new LCP compositions that can be used in the preparation of optical films as described above, which have significantly fewer of the aforementioned drawbacks. The present invention addresses that need.

[0004] Although several anisotropic LCP compounds are already known in the art, there remains a need to develop new LCP compounds with improved uniform polarization conversion over a wider wavelength range. Some examples of such anisotropic LCP compounds are disclosed in WO2012 / 147904, WO2016 / 104317, WO2017 / 043437 and JP2016 / 128403.

[0005] The present invention is directed to compositions comprising at least two anisotropic LCPs, LCP networks comprising said compositions, and optical and electro-optical devices, such as optical films, comprising said compositions or said networks.Optical films comprising such compositions have surprisingly been shown to be more effective at converting polarized light than optical films comprising only one LCP.

[0006] LCP films are generally produced by methods well known to those skilled in the art. This involves coating an organic solution of a crosslinkable LCP or LCP composition onto a substrate with an alignment layer or onto a substrate that has been pretreated by a rubbing technique. Alternatively, other aligning techniques for liquid crystals may be used. The organic solvent is then removed to obtain a well-aligned, solvent-free LCP layer, which is crosslinked to fix the liquid crystalline ordered structure. The desired optical performance of such films is highly dependent on several physical parameters that the anisotropic LCP material must simultaneously satisfy. Such properties are a low melting point or a low tendency to crystallize even when cooled below the melting point (supercooling), good solubility in organic solvents, good miscibility with other LCPs, good alignment properties on the alignment layer, and the ability to form an adjustable tilt with respect to the substrate plane essentially free of tilt domains and disclinations. Tilt domains are regions in an LCP film where the long axes of the LCP molecules form tilt angles with respect to the substrate plane of the same magnitude but opposite directions. Disclinations are the boundaries of adjacent tilt domains where LCP molecules with opposite tilt angles abut. These tilt domains and disclinations cause disruptions to the uniform appearance of the film and non-uniform optical performance.

[0007] Summary of the Invention It is a first object of the present invention to provide compositions comprising at least two anisotropic LCP compounds as described by formula (I), as well as formulations comprising at least one of said compounds and at least one additive and / or solvent.

[0008] It is a further object of the present invention to provide an optical film comprising said LCP composition and a method for preparing the same, the use of said optical film as a retardation film in achieving uniform polarization transformation, and devices comprising said optical film and their manufacture.

[0009] Detailed Description of the Invention A first aspect of the present invention provides a composition comprising at least two anisotropic liquid crystal compounds of formula (I): [ka] With the proviso that the two liquid crystal compounds are different and contain two different rings F, and ring F is selected from formula (IIa), (IIb) or (IIc) as follows:

[0010] A second aspect of the invention provides a formulation comprising the LCP composition of the first aspect of the invention and at least one solvent and / or additive.

[0011] The invention further provides an LCP network comprising said composition or LCP formulation, uses of said LCP composition or formulation or LCP network, and optical or electro-optical devices comprising said composition, formulation or network.

[0012] In the compounds of formula (I), ring F is selected from the group consisting of groups of formula (IIa), (IIb) or (IIc): [ka] wherein "*" represents a bond to a ring nitrogen atom of the compound of formula (I); and wherein Z is selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 12 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, wherein one or more carbon atoms are selected from the group consisting of -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a -, -CON-, -CO-R b , -NH-R c In the formula, R a is C1-C 12 is an alkyl group, R band R c are, independently of each other, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or an organic group having 2 to 30 carbon atoms containing at least one aromatic ring, or a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted cycloalkyl group having 3 to 12 carbon atoms.

[0013] Preferably, Z is selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

[0014] In the compounds of formula (I), (IIa), (IIb) and (IIc), R1, R2 and R3 are each independently hydrogen, C1-C 12 Straight or branched alkyl chain, C3-C 12 Alkenyl, C1-C 12 Alkoxy, C3-C 12 Alkenyloxy, -(CH2) m selected from the group consisting of -C(CH3)3, NO2, CN, COR, -COOR, -OCOR, -CONR'R, -NR'COR, OCOOR, -OCONR'R, -NR'COOR, -F, -Cl, -CF3 and -OCF3; During the ceremony, m is an integer between 0 and 12; R is hydrogen, C 1-18 Alkyl group, C with double bond at 3 or higher position 3-18 Alkenyl group, -(CH2) p -C-(CF3)3, CN and an unsubstituted or substituted phenyl ring, where the substituents on the phenyl ring are selected from the group consisting of a C1-C6 straight or branched alkyl chain, a C1-C6 alkoxy, -C-(CH3)3, halogen, -CF3, NO2, CN, COR''', -COOR''', -OCOR''', -CONR''R''', -NR''COR''', OCOOR''', -OCONR''R''', -NR''COOR''', -F, -Cl, -CF3 and -OCF3; During the ceremony, R″ is selected from the group consisting of hydrogen, lower alkyl, and lower alkenyl; R''' is hydrogen, C 1-18 Alkyl groups and C groups with double bonds at the 3rd or higher position 3-18 alkenyl groups; p is an integer between 0 and 12; R' is selected from the group consisting of hydrogen, lower alkyl, lower alkenyl, and lower alkoxy; During the ceremony, n is 0, 1, 2 or 3.

[0015] Preferably, R1, R2 and R3 are each independently selected from the group consisting of hydrogen, lower alkyl, lower alkenyl, lower alkoxy, lower alkenyloxy, -F, and -CF3.

[0016] Most preferably, R1, R2 and R3 are independently selected from the group consisting of hydrogen, methyl, methoxy, -F, -C-(CH3)3 and -CF3.

[0017] Y is selected from the group consisting of H or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

[0018] Rings C and D are each independently phenyl, biphenyl, naphthyl, cycloalkyl, preferably cyclohexyl, bicycloalkyl, preferably bicyclohexyl; [ka] is selected from the group consisting of:

[0019] Preferably, rings C and D are selected from cyclohexyl and phenyl rings.

[0020] In one embodiment of the invention, ring C is cyclohexyl and ring D is phenyl. In a further embodiment, rings C and D are both phenyl rings.

[0021] The substituents X1 and X2 are each independently hydrogen, C1-C 12 Substituted or unsubstituted straight or branched alkyl chains, C3-C 12 Substituted or unsubstituted straight or branched alkenyl chains and C1-C 12 alkoxy, where one or more carbon atoms are selected from the group consisting of -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a In the formula, R a is C1-C 12 or the substituents X1 and X2 are, independently of one another, represented by a group of formula (III): [ka]

[0022] In the group represented by formula (III), n is an integer between 0 and 24, where one or more carbon atoms are -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a In the formula, R a is C1-C 12 It is an alkyl group.

[0023] The substituent PG in the group represented by formula (III) is CH2=C(Ph)-, CH2=CW-COO-, CH2=CH-COO-Ph-, CH2=CW-CO-NH-, CH2=CH-O-, CH2=CH-OOC-, Ph-CH=CH-, CH2=CH-Ph-, CH2=CH-Ph-O-, R b -Ph-CH=CH-COO-, R b represents a polymerizable group selected from the group consisting of -OOC-CH=CH-Ph-O- and 2-W-epoxyethyl; where W represents H, Cl, Ph or lower alkyl, and R b represents lower alkyl, except that R bWhen attached to a phenylene group (-Ph-), it may also represent hydrogen or lower alkoxy. Preferably, PG represents an acrylate or methacrylate group.

[0024] Preferably, the substituents X1 and X2 are hydrogen, C1-C 12 Substituted or unsubstituted straight or branched alkyl chains, C3-C 12 Substituted or unsubstituted straight or branched alkenyl chains and C1-C 12 alkoxy (where rings C and D are, independently of each other, cyclohexyl or contain cyclohexyl).

[0025] Preferably, when rings C or D are, independently of one another, aromatic rings or contain an aromatic ring, more preferably when C or D are, independently of one another, phenyl rings or contain a phenyl ring, the group of formula (III) is [ka] wherein n has the same meaning as above, or their corresponding methacrylates.

[0026] The term "lower alkyl" means C 1-6 Examples of lower alkyl groups which may be present in the compounds of this invention include methyl, ethyl, propyl, butyl, pentyl, hexyl, and the like.

[0027] The term "lower alkenyl" refers to a C 3-6 Examples of lower alkenyl groups which may be present in the compounds of this invention include 2-propenyl, 3-butenyl, 3-isopentenyl, 4-pentenyl, 5-hexenyl, 4-isohexenyl, and the like.

[0028] The term "lower alkoxy" means 1-6Examples of lower alkoxy groups which may be present in the compounds of this invention include methoxy, ethoxy, propoxy, butoxy, pentoxy, hexoxy, and the like.

[0029] The term "lower alkenyloxy" refers to a C alkyl group having two or more double bonds. 3-6 Examples of lower alkenyloxy groups which may be present in the compounds of this invention include 2-propenyloxy, 3-butenyloxy, 4-pentenyloxy, 5-hexenyloxy, and the like.

[0030] The composition according to the first aspect of the present invention preferably contains at least one compound containing a ring F represented by formula (IIa).

[0031] The polymerizable anisotropic LCP compounds of the present invention can be readily prepared using procedures well known to those skilled in the art, a few non-limiting example procedures are provided in the Examples.

[0032] Starting materials are either commercially available or readily prepared and are well known to those skilled in the art.

[0033] Anisotropic LCP compound material as used within the context of this application shall mean a liquid crystal material comprising liquid crystal monomers and / or liquid crystal oligomers and / or liquid crystal polymers and / or crosslinked liquid crystals. When liquid crystal material comprises liquid crystal monomers, such monomers can typically be polymerized after anisotropy is created in the LCP material, for example by contact with an aligning layer or by rubbing. Polymerization can be initiated by heat treatment and / or exposure to actinic radiation (preferably including UV light). Anisotropic LCP material may comprise only one type of liquid crystal compound, but may also comprise additional polymerizable and / or non-polymerizable compounds, and not all of these compounds need to be liquid crystal compounds. When anisotropic LCP material comprises more than one anisotropic LCP represented by formula (I), this material is referred to as LCP composition in the context of the present invention. In the context of the present invention, LCP composition comprises at least two anisotropic LCP represented by formula (I). Furthermore, the LCP composition of the present invention may contain one or more additional LCP compounds, either the LCP compound shown in formula (I) or a different LCP compound not described by formula (I). It is also envisioned by the present invention that the LCP composition may also contain additional non-polymerizable compounds, such as dyes. In the case of optical films, anisotropic LCP monomers are applied on top of the photo-alignment layer or on top of the rubbed surface. After the alignment information of the photo-alignment layer or the rubbed surface is transferred to the LCP monomer, the monomers are polymerized and / or crosslinked to solidify the LCP material.

[0034] The LCP compositions of the present invention overcome the shortcomings of the prior art LCP compounds discussed above.

[0035] A further object of the invention relates to a formulation comprising at least two anisotropic LCP compounds (LCP compositions) of formula (I) and at least one solvent and / or additives, which may be selected from: antioxidants, initiators such as photoinitiators, accelerators, dyes, inhibitors, activators, fillers, chain transfer inhibitors, pigments, antistatic agents, flame retardants, thickeners, thixotropic agents, surfactants, viscosity modifiers, extender oils, plasticizers, tackifiers, catalysts, sensitizers, stabilizers, leveling agents, dispersants, polymeric binders and / or monomeric compounds that can be converted into polymeric binders by polymerization, or, in the case of emulsion paints and printing inks, dispersing aids, hydrophobizing agents, adhesives, flow improvers, defoamers, degassing agents, diluents, auxiliaries, colorants, dyes and pigments, cure inhibitors, chiral additives, isotropic or anisotropic fluorescent and / or non-fluorescent dyes, in particular dichroic dyes, and crosslinkers.

[0036] Solvents that may be used in the preparation of such liquid crystal compositions include, but are not limited to, acetone, cyclopentanone (CP), cyclohexanone (CH), methyl isobutyl ketone (MIBK), methyl ethyl ketone (MEK), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), N-ethylpyrrolidone, N-vinylpyrrolidone, N,N-dimethylacetamide (AN), tetrahydrofuran (THF), 1,3-dioxolane (DXG), ethylene glycol, dipropylene glycol, butyl carbitol, ethyl carbitol acetate, dipropylene glycol monomethyl ether, ethyl acetate (EA), 1-methoxy-2-propanol acetate (MPA), gamma-butyrolactone (BL), propylene glycol monoacetate, propylene glycol diacetate, dipropylene glycol monomethyl ether, dimethyl sulfoxide (DMSO). The most preferred solvents are cyclopentanone (CP), cyclohexanone (CH), methyl isobutyl ketone (MIBK), methyl ethyl ketone (MEK), ethyl acetate (EA), 1-methoxy-2-propanol acetate (MPA), 1,3-dioxolane (DXG), and dimethyl sulfoxide (DMSO).

[0037] The crosslinker is a compound containing one or more complementary reactive units or polymerizable groups P, such as hydroxyl, thiol or amino groups, through which it can react with the PG of the anisotropic LCP of the composition according to the invention. In order to maintain the liquid crystal phase, the crosslinker is preferably present in the claimed composition at no more than about 30 wt % based on the total weight of the polymerizable liquid crystal composition.

[0038] In the context of the present invention, suitable compounds containing thiols as reactive units or polymerizable groups P (called polythiols) may be any known in the art. As polythiols, any compound containing molecules with two or more thiol groups per molecule may be used. Polythiols have molecular weights ranging from about 50 to about 20,000.

[0039] Preferably, the polythiols are monomeric aliphatic polythiols, oligomeric polythiols, and polymeric polythiols.

[0040] Preferred polythiols relate to difunctional thiols, trifunctional thiols, tetrafunctional thiols or multifunctional thiols.

[0041] A preferred polymeric polythiol is polypropylene ether glycol bis(beta-mercaptopropionate), prepared, for example, by esterification of polypropylene ether glycol (e.g., Pluracol P201, Wyandotte Chemical Corp.) with beta-mercaptopropionic acid. Poly-alpha-mercaptoacetic acid esters or poly-beta-mercaptopropionic acid esters, especially trimethylpropane triesters or pentaerythritol tetraesters, are preferred.

[0042] Preferred alkylthiol functional compounds are, for example, 1,2-dimercaptoethane, 1,6-dimercaptohexane, decamethylenedithiol, etc. Thiol-terminated polysulfide resins may also be used.

[0043] Preferred aliphatic dithiols include 1,2-ethanedithiol, butanedithiol, 1,3-propanedithiol, 1,5-pentanedithiol, 2,3-dimercapto-1-propanol, dithioerythritol, 3,6-dioxa-1,8-octanedithiol, 1,8-octanedithiol, hexanedithiol, dithiodiglycol, pentanedithiol, decanedithiol, 2-methyl-1,4-butanedithiol, bis-mercaptoethylphenylmethane, 1,9-nonanedithiol (1,9-dimercaptononane), glycol dimercaptoacetate.

[0044] Preferred oligomeric dithiols include difunctional mercapto-functional urethane oligomers derived from end-capping moieties of hydroxyethyl mercaptan, hydroxypropyl mercaptan, dimercaptopropane, dimercaptoethane, as described in US Pat. No. 5,744,514 to Shustack.

[0045] Preferred trithiol functional compounds include trimethylolethane tris-mercaptopropionate, trimethylolpropane tris-mercaptopropionate (TMPTSH), trimethylolethane tris-mercaptoacetate, and trimethylolpropane tris-mercaptoacetate, glycerol tri(11-mercaptoundecanoate), trimethylolpropane tri(11-mercaptoundecate).

[0046] Preferred tetrafunctional thiols include pentaerythritol tetramercaptopropionate, pentaerythritol tetramercaptoacetate, and pentaerythritol tetra(11-mercaptoundecate).

[0047] In order to increase the mechanical strength or chemical resistance, or both, of the liquid crystal film, it is preferable to add a compound having two or more polymerizable groups to the composition. In order to increase the adhesion of the film to the substrate, it is preferable to add a crosslinker having a polar group at the side chain and / or at one end position to the composition.

[0048] Examples of such compounds are well known to those skilled in the art and are described in the prior art, for example in patent applications US 2017 / 0174992, WO 2018 / 099883 or WO 2008 / 077261.

[0049] These crosslinkers are usually photopolymerizable and include, for example, mono-, di- and polyfunctional compounds containing at least one olefinic double bond. Examples are vinyl esters of carboxylic acids (e.g., lauric acid, myristic acid, palmitic acid and stearic acid) and dicarboxylic acids (e.g., succinic acid, adipic acid), allyl and vinyl ethers and methacrylic and acrylic acid esters of monofunctional alcohols (e.g., lauryl alcohol, myristyl alcohol, palmityl alcohol and stearyl alcohol), and diallyl and divinyl ethers of difunctional alcohols (e.g., ethylene glycol and 1,4-butanediol).

[0050] Further examples are acrylic acid, methacrylic acid, maleic acid, fumaric acid and itaconic acid, styrene, nuclear-substituted styrene, acrylonitrile, vinyl chloride, vinylidene chloride, vinylpyridine, N-vinylpyrrolidone, vinylsulfonic acid, fatty acid vinyl esters, α,β-ethylenically unsaturated carboxylic acids, alkyl esters of (meth)acrylic acid in which the alkyl has 1 to 18 carbon atoms, hydroxyalkyl esters of (meth)acrylic acid in which the hydroxyalkyl has 1 to 18 carbon atoms, aminoalkyl esters of (meth)acrylic acid in which the aminoalkyl has 1 to 18 carbon atoms, and the like. p) Aminoalkyl esters of acrylic acid, ether oxygen-containing alkyl esters of (meth)acrylic acid in which the ether oxygen-containing alkyl has 3 to 18 carbon atoms, N-vinylacetamide, pt-butyl vinyl benzoate, N,N-dimethylaminovinyl benzoate, vinyl benzoate, vinyl pivalate, vinyl 2,2-dimethylbutanoate, vinyl 2,2-dimethylpentanoate, vinyl 2-methyl-2-butanoate, vinyl propionate, vinyl stearate, vinyl 2-ethyl-2-methylbutanoate, dicyclopentanyl Oxylethyl (meth)acrylate, isobornyloxylethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dimethyladamantyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, 2-acryloyloxyethyl succinate, 2-acryloyloxyethyl hexahydrophthalic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl-2-hydroxyethyl phthalic acid, 2 -acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, mono(meth)acrylate, polypropylene glycol (having a degree of polymerization of 2 to 100 and capped with a di(meth)acrylate ester or an alkyl group having 1 to 6 carbons), and mono(meth)acrylate ester of polyethylene glycol and copolymer of ethylene oxide and polypropylene oxide, which are non-liquid crystal polymerizable compounds that are monofunctional compounds.

[0051] Examples of difunctional compounds are 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, neopentyl glycol diacrylate, dimethyloltricyclodecane diacrylate, triethylene glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, tetraethylene glycol diacrylate, bisphenol A EO adduct diacrylate, bisphenol A glycidyl diacrylate, polyethylene glycol diacrylate and methacrylate.

[0052] Examples of trifunctional or higher functional polyfunctional compounds are pentaerythritol triacrylate, trimethylolpropane triacrylate, trimethylol EO-added triacrylate, trisacryloyloxyethyl phosphate, tris(acryloyloxyethyl)isocyanurate, alkyl-modified dipentaerythritol triacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, pentaerythritol tetraacrylate, alkyl-modified dipentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, dipentaerythritol monohydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, pentaerythritol tri(meth)acrylate, dipenta ... tris(meth)acrylate, trimethylolpropane tri-(meth)acrylate, trimethylol EO adduct tri(meth)acrylate, tris(meth)acryloyloxyethyl phosphate, tris(meth)acryloyloxyethyl isocyanurate, alkyl modified dipentaerythritol tri(meth)acrylate, EO modified trimethylolpropane tri(meth)acrylate, PO modified trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, alkyl modified dipentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol monohydroxypentamethacrylate, and alkyl modified dipentaerythritol pentamethacrylate.

[0053] The present invention further provides an LCP network comprising a composition or formulation according to the first and second aspects. The network may contain crosslinked and non-crosslinked anisotropic LCPs according to formula (I).

[0054] The present invention relates to an optical film comprising at least one of the anisotropic LCP compounds or compositions according to the present invention. An example of an optical film is a circular polarizer film used as an anti-reflection film produced by combining the optical film according to the present invention with a linear polarizer.

[0055] The anisotropic LCP compound or a composition comprising an anisotropic LCP compound can be applied onto a support. The support can be rigid or flexible and can have any form or shape. In principle, the support can be made of any material. Preferably, the support comprises plastic, glass or metal, or is a silicon wafer. If the support is flexible, the support is preferably a plastic or metal foil. Preferably, the surface of the support is flat. In some applications, the support can include topographical surface structures, such as microstructures, such as microlenses or microprisms, or structures that show abrupt changes in shape, such as rectangular structures. Preferably, the support is transparent. The support can also be treated before coating with the anisotropic LCP compound according to the present invention.

[0056] The support may be moving during deposition of the anisotropic LCP compound or the composition comprising the anisotropic LCP compound.For example, the layer of the LCP mixture may be produced in a continuous roll-to-roll process by depositing the material composition on a moving flexible foil, preferably plastic or metal.The resulting film may then be wound on a roll together with the support foil, or the film may be peeled off from the support, and the film may then be wound as a free-standing film without the support.

[0057] The support may have additional layers, such as photo-aligning layers, organic layers, dielectric layers or metal layers. The layers may have various functions, for example, the organic layer may be coated as a primer layer to enhance the compatibility of the material to be coated with the support. The metal layer may be used as an electrode or may have the function of a reflector, for example, when used in an electro-optical device such as a display. The support may also be an optical element or device with a specific function, such as a substrate for an LCD, which may include thin film transistors, electrodes or color filters. In another example, the support is a device that includes an OLED layer structure. The support may also be a polarizer, such as a polarizing film or sheet polarizer, a reflective polarizer, such as the commercially available Vikuity™ DBEF film.

[0058] In the context of the present invention, a "photoaligning layer" is made of a material that can induce anisotropic properties when exposed to aligning light, i.e., a photoalignable material. In addition, the term "photoaligning layer" also refers to a layer that is aligned by exposure to aligning light. In the present invention, the induced anisotropy must be such that it provides alignment capability to adjacent layers that contain, for example, anisotropic LCP compounds of formula (I). The term "alignment direction" refers to the preferred direction induced in the adjacent layer, for example, the alignment direction is the direction in which the LCP compounds are aligned.

[0059] The photoalignable material includes photoalignable moieties that exhibit a preferred orientation when exposed to aligning light, thus creating anisotropic properties. Such photoalignable moieties preferably have anisotropic absorption properties. Typically, such moieties exhibit absorption within a wavelength range of 230-500 nm. Preferably, the photoalignable moieties exhibit light absorption within a wavelength range of 300-450 nm, more preferably within a wavelength range of 310-380 nm.

[0060] Preferably, the photoalignable moiety has a carbon-carbon, carbon-nitrogen, or nitrogen-nitrogen double bond.

[0061] For example, the photoalignable moiety can be a substituted or unsubstituted azo dye, anthraquinone, coumarin, melissyanin, 2-phenylazothiazole, 2-phenylazobenzthiazole, stilbene, cyanostilbene, fluorostilbene, cinnamonitrile, chalcone, cinnamate, cyanocinnamate, stilbazolium, 1,4-bis(2-phenylethylenyl)benzene, 4,4'-bis(arylazo)stilbene, perylene, 4,8-diamino-1,5-naphthoquinone dye, aryloxycarboxylic acid derivatives, aryl esters, N-arylamides, polyimides, diaryl ketones having a ketone moiety or ketone derivative attached to two aromatic rings, such as substituted benzophenones, benzophenone imines, phenylhydrazones, and semicarbazones.

[0062] The preparation of the above-listed anisotropic absorbent materials is well known as shown, for example, in U.S. Pat. No. 4,565,424 to Hoffman et al., U.S. Pat. No. 4,401,369 to Jones et al., U.S. Pat. No. 4,122,027 to Cole, Jr. et al., U.S. Pat. No. 4,667,020 to Etzbach et al., and U.S. Pat. No. 5,389,285 to Shannon et al.

[0063] Preferably, the photoalignable moiety comprises an arylazo, a poly(arylazo), a stilbene, a cyanostilbene, a cinnamate, or a chalcone.

[0064] The photoalignable material may be, inter alia, a monomer, an oligomer, or a polymer. The photoalignable moieties may be, for example, covalently bound within the backbone or side chains of a polymer or oligomer, or may be part of a monomer or other compound that is not polymerizable. The photoalignable material may also be a copolymer that includes different types of photoalignable moieties, or that includes side chains with and without photoalignable moieties.

[0065] Polymers are understood to mean, for example, polyacrylates, polymethacrylates, polyimides, polyurethanes, polyamic acids, polymaleimides, poly-2-chloroacrylates, poly-2-phenylacrylates; unsubstituted or C1-C6 alkyl substituted polyacrylamides, polymethacrylamides, poly-2-chloroacrylamides, poly-2-phenylacrylamides, polyethers, polyvinyl ethers, polyesters, polyvinyl esters, polystyrene derivatives, polysiloxanes, linear or branched alkyl esters of polyacrylic acid or polymethacrylic acid; polyphenoxyalkylacrylates, polyphenoxyalkylmethacrylates, polyphenylalkylmethacrylates with alkyl residues of 1 to 20 carbon atoms; polyacrylonitriles, polymethacrylonitriles, cycloolefin polymers, polystyrene, poly-4-methylstyrene, or mixtures thereof.

[0066] The photoalignable material may also include photosensitizers, such as ketocoumarins and benzophenones.

[0067] Further preferred photoalignable monomers or oligomers or polymers are described in US Pat. No. 5,539,074, US Pat. No. 6,201,087, US Pat. No. 6,107,427, US Pat. No. 6,632,909 and US Pat. No. 7,959,990.

[0068] Alignment of LCP can be achieved by any other known means for aligning liquid crystal. For example, the support can have an aligning surface, which means that the surface has the ability to align liquid crystal. The support can be pre-aligned without further processing. For example, when a plastic substrate is used as the support, it can be aligned on the surface due to the manufacturing method, such as extrusion or stretching of the substrate. It is also possible to brush or rub the support to generate alignment ability, or to imprint directional microstructures.

[0069] The steps of polymerizing the LCP compound and exposing it to the aligning light can be in any order. Polymerization can be initiated before or after exposure to the aligning light. Alternatively, polymerization and exposure can occur simultaneously.

[0070] The LCP composition or formulation may be applied to the support by any suitable method, such as extrusion, casting, molding, 2D or 3D printing or coating. Suitable coating methods are, for example, spin coating, blade coating, knife coating, kiss roll coating, die coating, dipping, brushing, casting with a bar, roller coating, flow coating, wire coating, spray coating, dip coating, curtain coating, air knife coating, reverse roll coating, gravure coating, metering rod (Meyer bar) coating, slot die (extrusion) coating, roller coating, flexographic coating. Suitable printing methods include silk screen printing, relief printing, such as flexographic printing, jet printing, intaglio printing, such as direct gravure printing or offset gravure printing, lithographic printing, such as offset printing, or stencil printing, such as screen printing.

[0071] The compositions and formulations according to the present invention exhibit improved retardation patterns compared to prior art compositions and formulations containing only one LCP compound.

[0072] The present invention will now be described with reference to the following non-limiting examples, which are provided for illustrative purposes only. Variations to these examples which fall within the scope of the invention will be apparent to those of ordinary skill in the art. EXAMPLES

[0073] The following examples are provided to further illustrate and facilitate the understanding of the present invention and are not intended to limit the present invention in any manner.

[0074] Example 1: Synthesis of [2-[(E)-[methyl(quinoxalin-2-yl)hydrazono]methyl]-4-(4-propylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 1 Synthesis of (3-formyl-4-hydroxy-phenyl) 4-propylcyclohexanecarboxylate: To a solution of 2,5-dihydroxybenzaldehyde (1.38 g, 10 mmol), trans-4-propylcyclohexane-carboxylic acid (1.79 g, 10.5 mmol) and 4-dimethylaminopyridine (DMAP) (122 mg, 1 mmol) in dry dichloromethane (20 mL) was added 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) (1.94 mL, 11 mmol) slowly. The reaction mixture was stirred at ambient temperature for 22 h. The reaction mixture was quenched with saturated aqueous sodium bicarbonate and extracted with dichloromethane. The organic phase was washed with brine, dried over anhydrous sodium sulfate and the solvent was removed under reduced pressure. The residue was purified by silica gel flash column chromatography using ethyl acetate / hexane to give the title compound as a yellow solid (1.31 g, 45%). 1H-NMR (400 MHz, CDCl3) δ 10.90 (s, 1H), 9.85 (s, 1H), 7.31 (d, J = 2.7 Hz, 1H), 7.23 (dd, J = 9.1, 2.7 Hz, 1H), 6.99 (d, J = 9.1 Hz, 1H), 2.44-2.52 (m, 1H), 2.11-2.15 (m, 2H), 1.86-1.90 (m, 2H), 1.50-1.57 (m, 2H), 1.29-1.39 (m, 3H), 1.17-1.23 (m, 2H), 0.97-1.04 (m, 3H), 0.87-0.92 (m, 3H)

[0075] Synthesis of [2-formyl-4-(4-propylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate: To a solution of (3-formyl-4-hydroxy-phenyl) 4-propylcyclohexanecarboxylate (1.3 g, 4.5 mmol), 4-(6-acryloyloxy-hex-1-yloxy)benzoic acid (1.38 g, 4.70 mmol) and 4-dimethylaminopyridine (DMAP) (55 mg, 0.45 mmol) in dry dichloromethane (9 mL) was added 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) (0.87 mL, 4.93 mmol). The reaction mixture was stirred at ambient temperature for 5 h. The reaction mixture was quenched with saturated aqueous sodium bicarbonate and extracted with ethyl acetate. The organic phase was washed with brine, dried over anhydrous sodium sulfate and the solvent was removed under reduced pressure. The residue was purified by silica gel flash column chromatography using ethyl acetate / hexane to give the title compound as a beige oil (2.73 g) containing some impurities, which was used in the next reaction without further purification.

[0076] Synthesis of [2-[(E)-[methyl(quinoxalin-2-yl)hydrazono]methyl]-4-(4-propylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 1: (±)10-Camphorsulfonic acid (105 mg, 0.45 mmol) was added to a solution of [3-formyl-4-(4-propylcyclohexanecarbonyl)oxy-phenyl] 4-(6-prop-2-enoyloxyhexoxy)benzoate (2.73 g, 4.5 mmol), 1-methyl-1-quinoxalin-2-yl-hydrazine (0.82 g, 4.7 mmol), and 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical (TEMPO-OH) (9 mg, 0.05 mmol) in anhydrous tetrahydrofuran (45 mL) under nitrogen atmosphere. The resulting solution was stirred at ambient temperature for 24 h. The reaction mixture was quenched with saturated aqueous sodium bicarbonate and extracted with dichloromethane. The organic phase was washed with brine, dried over anhydrous sodium sulfate, and the solvent was removed under reduced pressure. After recrystallization from dichloromethane / hexane, the title compound was obtained as a grey solid (1.61 g, 50%). 1 H-NMR (400 MHz, DMSO-d6) δ 9.39 (s, 1H), 8.14 (d, J = 9.1 Hz, 2H), 7.90-7.92 (m, 2H), 7.85-7.86 (m, 1H), 7.75-7.77 (m, 1H), 7.67-7.71 (m, 1H), 7.52-7.56 (m, 1H), 7.39 (d, J = 8.7 Hz, 1H), 7.20 (dd, J = 8.7, 2.7 Hz, 1H), 7.12 (d, J = 8.7 Hz, 2H), 6.32 (dd, J = 17.2, 1.6 Hz, 1H), 6.17 (dd, J = 17.4, 10.5 Hz, 1H), 5.93 (dd, J = 10.3, 1.6 Hz, 1H), 4.07-4.13 (m, 4H), 3.62 (s, 3H), 2.11-2.15 (m, 2H), 1.72-1.84 (m, 4H), 1.61-1.68 (m, 2H), 1.37-1.54 (m, 7H), 1.27-1.35 (m, 3H), 1.16-1.21 (m, 2H), 0.95-1.04 (m, 2H), 0.87 (t, J = 7.1 Hz, 3H)

[0077] Example 2: Synthesis of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2 Synthesis of [3-formyl-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate: Oxalyl chloride (2.5 mL, 29 mmol) was added dropwise to a solution of 4-(6-acryloyloxy-hex-1-yloxy)benzoic acid (6.98 g, 24 mmol) in 48 mL of anhydrous toluene, 4 mg of 4-methoxyphenol and 1 mL of anhydrous DMF at 45 °C. After 2 h, the reaction mixture was cooled to 0 °C and added dropwise to a solution of 2,5-dihydroxybenzaldehyde (1.5 g, 11 mmol) in 40 mL of anhydrous DMA and N,N-dimethylcyclohexylamine (7.8 g, 52 mmol) at 0-5 °C. The reaction mixture was stirred overnight at ambient temperature. The organic solution was quenched by the addition of 15 mL of water, extracted with dichloromethane, washed successively with water, brine, dried over sodium sulfate and concentrated under vacuum. After recrystallization from dichloromethane / methanol, the title compound was obtained as a white solid (4.19 g, 56%).

[0078] Synthesis of 9-amino-3-methylcarbazole: To a suspension of 3-methylcarbazole (4.8 g, 26.5 mmol) and potassium hydroxide (11.9 g, 212 mmol) in dry DMF (53 mL) was added a solution of hydroxylamine-O-sulfonic acid (HOSA) (5.99 g, 53 mmol) in dry DMF (106 mL) dropwise at 0° C. for 65 min. After addition, the reaction mixture was quenched with water and extracted with ethyl acetate / hexane=3 / 1. The organic phase was washed successively with water, brine, dried over anhydrous sodium sulfate, and the solvent was removed under reduced pressure to give the title compound as a beige solid (5.1 g, 98%). 1H-NMR (400 MHz, DMSO-d6) δ 8.04 (d, J = 7.8 Hz, 1H), 7.88 (s, 1H), 7.54 (d, J = 8.2 Hz, 1H), 7.47 (d, J = 8.2 Hz, 1H), 7.41 (td, J = 7.7, 1.1 Hz, 1H), 7.26 (dd, J = 8.2, 1.4 Hz, 1H), 7.12 (t, J = 7.5 Hz, 1H), 5.76 (s, 2H), 2.46 (s, 3H)

[0079] Synthesis of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2: (±)10-Camphorsulfonic acid (18.6 mg, 0.08 mmol) was added to a solution of the described [3-formyl-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate (0.57 g, 0.83 mmol) and 9-amino-3-methyl-carbazole (0.20 g, 1 mmol) in 8 mL of dry tetrahydrofuran under nitrogen atmosphere. The resulting solution was stirred at ambient temperature for 17 hours. After completion of the reaction, the reaction mixture was quenched with saturated aqueous sodium bicarbonate solution and extracted twice with dichloromethane. The organic phase was washed with brine, dried over anhydrous sodium sulfate and the solvent was removed under reduced pressure. After recrystallization from dichloromethane / hexane, the title compound was obtained as a beige solid (0.42 g, 59%). 1H-NMR (400 MHz, DMSO-d6) δ 9.14 (s, 1H), 8.23 ​​(d, J = 9.1 Hz, 2H), 8.09-8.15 (m, 4H), 7.96 (s, 1H), 7.70 (d, J = 7.3 Hz, 1H), 7.64 (d, J = 8.2 Hz, 1H), 7.48-7.55 (m, 2H), 7.22-7.30 (m, 2H), 7.10-7.18 (m, 5H), 6.29-6.34 (m, 2H), 6.13-6.21 (m, 2H), 5.90-5.95 (m, 2H), 4.08-4.14 (m, 8H), 2.43 (s, 3H), 1.76-1.79 (m, 4H), 1.59-1.68 (m, 4H), 1.40-1.49 (m, 8H); MALDI-TOF (CHCA) 887.35 (M + +Na)

[0080] Example 3: Synthesis of [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 3 Synthesis of 1-(1,3-benzothiazol-2-yl)-1-hexyl-hydrazine: A four-neck reactor was charged with 2-hydrazinobenzothiazole (3.5 g, 0.020 mol) and 20 mL of DMF. NaOH (1.25 g, 0.030 mol) was added slowly under nitrogen flow. After addition of 1-bromohexane (4.05 g, 0.024 mol), the mixture was heated to 60° C. for 4 h. After completion of the reaction, the reaction mixture was cooled to 25° C. and added to 200 mL of water and 100 mL of heptane. The precipitate was filtered off to give 2.45 g as a white solid.

[0081] Synthesis of (3-formyl-4-hydroxy-phenyl) 4-butylcyclohexanecarboxylate: A solution of DCC (22.9 g, 0.11 mol) in 60 mL of dichloromethane was added dropwise to a cooled mixture of 2,5-dihydroxybenzaldehyde (13.95 g, 0.1 mol), trans-4-butylcyclohexanecarboxylic acid (19.55 g, 0.105 mol) and 4-dimethylaminopyridine (1.25 g, 0.01 mol) in 180 mL of dichloromethane. The reaction mixture was stirred overnight at ambient temperature. The mixture was filtered through a Hyflo® super Cell® and the solution was concentrated under vacuum. The residue was dissolved in 250 mL of methanol and then the solution was cooled to 0° C. The precipitate was filtered off and dried under vacuum at 40° C. to give 20.3 g of an off-white solid.

[0082] Synthesis of [4-(4-butylcyclohexanecarbonyl)oxy-2-formyl-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate: DCC (12.5 g, 0.060 mol) was added to a cooled mixture of (3-formyl-4-hydroxy-phenyl) 4-butylcyclohexanecarboxylate (15.2 g, 0.050 mol), 4-(6-prop-2-enoyloxyhexoxy)benzoic acid (16.95 g, 0.055 mol) and 4-dimethylaminopyridine (0.6 g, 0.005 mol) in 175 mL of dichloromethane. The reaction mixture was stirred overnight at ambient temperature and then filtered through a Hyflo® super Cell®. The resulting solution was concentrated under vacuum. The residue was dissolved in 350 mL of methanol and then the solution was cooled to 0° C. The precipitate was filtered off and dried under vacuum at 40° C. to give 20.1 g of a white solid.

[0083] Synthesis of [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 3: DL-10-Camphorsulfonic acid (0.40 g, 0.0016 mol) was added to a yellow solution of [4-(4-butylcyclohexanecarbonyl)oxy-2-formyl-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate (9.35 g, 0.016 mol) and 1-(1,3-benzothiazol-2-yl)-1-hexyl-hydrazine (4.75 g, 0.019 mol) dissolved in 120 mL of THF. The mixture was stirred overnight at room temperature. After addition of ethyl acetate, the solution was washed with a 5 wt% solution of sodium bicarbonate, dried over sodium sulfate and concentrated under vacuum. After recrystallization from methanol, 11.2 g of the title compound was obtained as an off-white solid. 1 H NMR (400 MHz, DMSO-d6) δ: 8.15 (d, 2H), 7.81 (m, 2H), 7.58 (m, 2H), 7.42 (d, 1H), 7.32 (t, 1H), 7.25 (dd, 1H), 7.14 (m, 3H), 6.334 (dd, 1H), 6.18 (dd, 1H), 5.93 (d, 1H), 4.19 (t, 2H), 4.12 (m, 4H), 2.58 (tt, 1H), 2.12 (d, 2H), 1.92-0.80 (m, 32H), 0.72 (t, 3H)

[0084] Example 4: Synthesis of [3-[(E)-(3,6-dimethylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 4 Synthesis of 9-amino-3,6-dimethylcarbazole: To a suspension of 3,6-dimethylcarbazole (1.88 g, 9.6 mmol) and potassium hydroxide (8.6 g, 154 mmol) in dry DMF (19 mL) was added a solution of hydroxylamine-O-sulfonic acid (HOSA) (2.17 g, 19.2 mmol) in dry DMF (38 mL) dropwise at 0° C. for 10 min. The reaction mixture was stirred at room temperature, quenched with water, and extracted with a 1:2 mixture of ethyl acetate / hexane. The organic phase was washed successively with water, brine, dried over anhydrous sodium sulfate, and the solvent was removed under reduced pressure. The residue was purified by silica gel flash column chromatography using a 1:4 mixture of ethyl acetate / hexane to give the title compound as a white solid (1.7 g, 85%). 1 H-NMR (400 MHz, DMSO-d6) δ 7.82 (s, 2H), 7.42 (d, J = 8.2 Hz, 2H), 7.23 (dd, J = 8.2, 1.4 Hz, 2H), 5.70 (s, 2H), 2.45 (s, 6H)

[0085] Synthesis of [3-formyl-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate: Oxalyl chloride (2.5 mL, 29 mmol) was added dropwise to a solution of 4-(6-acryloyloxy-hex-1-yloxy)benzoic acid (6.98 g, 24 mmol) in 48 mL of anhydrous toluene, 4 mg of 4-methoxyphenol and 1 mL of anhydrous DMF at 45 °C. After 2 h, the reaction mixture was cooled to 0 °C and added dropwise to a solution of 2,5-dihydroxybenzaldehyde (1.5 g, 11 mmol) in 40 mL of anhydrous DMA and N,N-dimethylcyclohexylamine (7.8 g, 52 mmol) at 0-5 °C. The reaction mixture was stirred overnight at ambient temperature. The organic solution was quenched by the addition of 15 mL of water, extracted with dichloromethane, washed successively with water, brine, dried over sodium sulfate and concentrated under vacuum. After recrystallization from dichloromethane / methanol, the title compound was obtained as a white solid (4.19 g, 56%).

[0086] Synthesis of [3-[(E)-(3,6-dimethylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate: (±)10-Camphorsulfonic acid (46.5 mg, 0.2 mmol) was added to a solution of [3-formyl-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate (1.37 g, 2.0 mmol) and 9-amino-3,6-dimethylcarbazole (0.50 g, 2.4 mmol) in 20 mL of dry tetrahydrofuran under nitrogen atmosphere. The resulting solution was stirred at ambient temperature for 16 h. After completion of the reaction, the reaction mixture was quenched with saturated aqueous sodium bicarbonate solution and extracted with dichloromethane. The organic phase was washed with brine, dried over anhydrous sodium sulfate and the solvent was removed under reduced pressure. After recrystallization from dichloromethane / hexane, the title compound was obtained as a beige solid (0.541 g, 74%). 1H-NMR (400 MHz, DMSO-d6) δ 9.08 (s, 1H), 8.22 (d, J = 9.1 Hz, 2H), 8.14 (d, J = 8.7 Hz, 2H), 8.12 (d, J = 2.7 Hz, 1H), 7.90 (s, 2H), 7.59 (d, J = 8.2 Hz, 2H), 7.53 (d, J = 8.7 Hz, 1H), 7.48 (dd, J = 8.7, 2.7 Hz, 1H), 7.18 (d, J = 8.7 Hz, 2H), 7.14 (d, J = 8.7 Hz, 2H), 7.08 (dd, J = 8.7, 1.4 Hz, 2H), 6.29-6.34 (m, 2H), 6.12-6.21 (m, 2H), 5.90-5.95 (m, 2H), 4.06-4.15 (m, 8H), 2.42 (s, 6H), 1.77 (td, J = 12.8, 6.6 Hz, 4H), 1.59-1.68 (m, 4H), 1.41-1.52 (m, 8H); MALDI-TOF (CHCA) 901.35 (M + +Na)

[0087] Example 5: Preparation of alignment layer using photo-alignment material A glass substrate was spin-coated with the photoalignment composition (solid content of photoaligning polymer: 2% in cyclopentanone, as described in the application example on page 40 of patent publication WO2012 / 085048). The film was dried at 80 °C for 30 s, and the resulting film thickness was about 100 nm. The film was then exposed to an aligning light of parallel linearly polarized UV (LPUV) light (280-320 nm) at 250 mJ / cm. 2 The plane of polarization was at 0° to a reference edge on the substrate.

[0088] Example 6: A 10.0 wt % solution of composition 1 was prepared as follows: 5.618 wt % of [3-[(E)-[methyl(quinoxalin-2-yl)hydrazono]methyl]-4-(4-propylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 1, 0.0075 wt % of the inhibitor 2,6-di-tert-butyl-4-methylphenol (to prevent premature polymerization), 0.45 wt % of the photoinitiator Irgacure® Oxe 02 (BASF), 0.45 wt % of [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.225 wt % of Tego® flow. 425, 8.25 wt% of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2 was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. The coating liquid was applied by spin coating on a glass plate with the alignment layer of Example 5 to form a liquid crystal film. The film was dried on a temperature-controlled hot plate at 105°C for 5 minutes. The sample was cooled to room temperature and then photopolymerized by irradiating UV light using a mercury lamp under a N2 atmosphere at room temperature for approximately 2 minutes to fix the alignment state of the liquid crystal.

[0089] The alignment quality of the liquid crystal in the film is checked by placing the film between two crossed polarizers and adjusting to obtain a dark state. If the dark state shows no defects and the liquid crystal is well aligned, the alignment quality is defined as very good. If the dark state has light leakage due to non-uniform alignment of the liquid crystal, the alignment quality is defined as good. If the dark state has light leakage with some areas of crystallization, the alignment quality is defined as fair. If there is no dark state and the liquid crystal is not aligned, the alignment quality is defined as poor. The obtained film of Example 6 showed very good alignment quality.

[0090] Example 7: A 15.0 wt% solution of composition 2 was prepared as follows: 9.3675 wt% [3-[(E)-[methyl(quinoxalin-2-yl)hydrazono]methyl]-4-(4-propylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 1, 0.0075 wt% inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.45 wt% photoinitiator Irgacure® Oxe 02, 0.45 wt% [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.225 wt% Tego® flow 425, 4.5 wt% of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2 was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. A film was prepared as described in Example 6 and dried on a temperature-controlled hotplate at 105°C for 5 minutes. The resulting film showed very good alignment quality.

[0091] Example 8: A 26.0 wt% solution of composition 3 was prepared as follows: 21.4370 wt% [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate, 0.013 wt% inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.45 wt% photoinitiator Irgacure® Oxe 03, 0.78 wt% [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.390 wt% Tego® flow 425, 2.6 wt% of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. A film was prepared as described in Example 6 and dried on a temperature controlled hotplate at 68°C for 2 minutes. The resulting film showed very good alignment quality.

[0092] Example 9: A 35.0 wt% solution of composition 4 was prepared as follows: 9.2075 wt% [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate, 0.0175 wt% inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.7 wt% photoinitiator Irgacure® Oxe 03, 1.05 wt% [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.525 wt% Tego® flow. 425, 3.5 wt% of [3-[(E)-(3,6-dimethylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. A film was prepared as described in Example 6 and dried on a temperature controlled hotplate at 70°C for 2 minutes. The resulting film showed very good alignment quality.

[0093] Example 10: A 15.0 wt% solution of Composition 5 was prepared as follows: 11.2425 wt% [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate, 0.0075 wt% inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.3 wt% photoinitiator Irgacure® Oxe 03, 0.3 wt% [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.150 wt% Tego® flow 425, 3.0 wt% of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2 was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. A film was prepared as described in Example 6 and dried on a temperature-controlled hotplate at 80°C for 5 minutes. The resulting film showed very good alignment quality.

[0094] Example 11: A 15.0 wt% solution of Composition 6 was prepared as follows: 9.7425 wt% [2-[(E)-[1,3-benzothiazol-2-yl(hexyl)hydrazono]methyl]-4-(4-butylcyclohexanecarbonyl)oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate, 0.0075 wt% inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.3 wt% photoinitiator Irgacure® Oxe 03, 0.3 wt% [3-(3-sulfanylpropanoyloxy)-2,2-bis(3-sulfanylpropanoyloxymethyl)propyl]3-sulfanylpropanoate, 0.150 wt% Tego® flow. 425, 4.5 wt% of [3-[(E)-(3-methylcarbazol-9-yl)iminomethyl]-4-[4-(6-prop-2-enoyloxyhexoxy)benzoyl]oxy-phenyl]4-(6-prop-2-enoyloxyhexoxy)benzoate compound 2 was mixed in cyclohexanone and thoroughly stirred at room temperature until the solid was completely dissolved. A film was prepared as described in Example 6 and dried on a temperature-controlled hotplate at 77°C for 5 minutes. The resulting film showed very good alignment quality.

[0095] Example 12: Comparative Example A comparative 30.0 wt% solution is prepared as follows: 28.05 wt% of compound 2, 0.15 wt% of inhibitor 2,6-di-tert-butyl-4-methylphenol, 0.9 wt% of photoinitiator Irgacure® Oxe 03 and 0.9 wt% of Tinuvin 123 are mixed in cyclohexanone and thoroughly stirred at room temperature until the solids are completely dissolved. A film is prepared as described in Example 6 and dried on a temperature-controlled hotplate at 105°C for 5 minutes. The resulting film shows very good alignment quality.

[0096] Example 13: The retardation of the samples described in Examples 6 to 11 was measured with an ellipsometer. Table 1 shows the results of the retardation of Compositions 1 and 2. Table 2 shows the results of the retardation of Compositions 3 to 6. 450 The value represents the retardation of the film at a wavelength of 450 nm, Re 550 The value represents the retardation of the film at a wavelength of 550 nm, Re 650 The values ​​represent the retardation of the film at a wavelength of 650 nm.

[0097] [Table 1]

[0098] [Table 2]

[0099] To improve color, Re 650 / Re 550 It is preferable that the value of Re is higher than 1.00 and less than 1.2. 450 / Re 550 The value is preferably less than 0.90. Table 1 shows the results of retardation properties of liquid crystal compositions 1 and 2 containing one LCP from group IIa and one LCP from group IIb. Table 2 shows the results of retardation properties of liquid crystal compositions 3 to 6 containing one LCP from group IIa and one LCP from group IIc.

[0100] Re of films from compositions 2 and 6 650 / Re 550 is the Re of the liquid crystal composition of the comparative example 650 / Re 550 significantly higher than Re 650 / Re 550 The maximum value of Re is 1.03. 450 / Re 550 The value is the Re 450 / Re 550Compared to the values, it is significantly reduced in compositions 2 to 6, reaching values ​​of 0.83 to 0.90. The new compositions according to the present invention show improved retardation properties compared to the comparative examples containing only one LCP compound.

Claims

1. Formula (I): [C6] [In the formula, Rings C and D are each independently phenyl, biphenyl, naphthyl, cycloalkyl, bicyclohexyl, [C7] selected from the group consisting of: Ring E is selected from the group consisting of phenyl, biphenyl, and naphthyl; Ring F is represented by formula (IIa), (IIb) or (IIc): [C8] {wherein "*" represents a bond to the nitrogen atom of the compound of formula (I)} is selected from the group consisting of the groups represented by X 1 and X 2 are each independently hydrogen, C 1 -C 12 Substituted or unsubstituted straight or branched alkyl chains, C 3 -C 12 Substituted or unsubstituted straight or branched alkenyl chain and C 1 -C 12 alkoxy, where one or more carbon atoms are selected from the group consisting of -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a may be replaced by -, -CON-, a is C 1 -C 12 is an alkyl group; or X 1 and X 2 are each independently represented by the formula (III): [C9] wherein n is an integer between 0 and 24; and wherein one or more carbon atoms are -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a may be replaced by -, -CON-, a is C 1-C 12 is an alkyl group; and PG is CH 2 =C(Ph)-, CH 2 =CW-COO-, CH 2 =CH-COO-Ph-, CH 2 =CW-CO-NH-, CH 2 =CH-O-, CH 2 =CH-OOC-, Ph-CH=CH-, CH 2 =CH-Ph-, CH 2 =CH-Ph-O-, R b -Ph-CH=CH-COO-, R b represents a polymerizable group selected from the group consisting of -OOC-CH=CH-Ph-O- and 2-W-epoxyethyl; where W represents H, Cl, Ph or lower alkyl, and R b represents lower alkyl, provided that R b When attached to a phenylene group (-Ph-), it may also represent hydrogen or lower alkoxy. Represented by a group represented by: Y is selected from the group consisting of H or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 1 , R 2 and R 3 are each independently hydrogen, C 1 -C 12 Linear or branched alkyl chain, C 3 -C 12 Alkenyl, C 1 -C 12 Alkoxy, C 3 -C 12 Alkenyloxy, -(CH 2 ) m -C(CH 3 ) 3 , NO 2 , CN, COR, -COOR, -OCOR, -CONR'R, -NR'COR, OCOOR, -OCONR'R, -NR'COOR, -F, -Cl, -CF 3 and -OCF 3 selected from the group consisting of: During the ceremony, m is an integer between 0 and 12; R is hydrogen, C 1-18 Alkyl group, C having a double bond at the 3rd or higher position 3-18 Alkenyl group, -(CH 2 ) p -C-(CF 3 ) 3 , CN and an unsubstituted or substituted phenyl ring, wherein the substituents on the phenyl ring are selected from the group consisting of C 1 -C 6 Linear or branched alkyl chain, C 1 -C 6 Alkoxy, -C-(CH 3 ) 3 , halogen, -CF 3 , NO 2 , CN, COR''', -COOR''', -OCOR''', -CONR''', -NR'''COR''', OCOOR''', -OCONR'R''', -NR'''COOR''', -F, -Cl, -CF 3 and -OCF 3 selected from the group consisting of: During the ceremony, R″ is selected from the group consisting of hydrogen, lower alkyl, and lower alkenyl; R''' is hydrogen, C 1-18 Alkyl groups and C groups having a double bond at the 3rd or higher position 3-18 alkenyl groups; p is an integer between 0 and 12; R' is selected from the group consisting of hydrogen, lower alkyl, lower alkenyl, and lower alkoxy; During the ceremony, n is 0, 1, 2 or 3; Z is selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 12 carbon atoms, and a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, wherein one or more carbon atoms are selected from the group consisting of -O-, -COO-, -OCO-, -OOC-, -O(CO)O-, -N-, -NR a -, -CON-, -CO-R b , -NH-R c In the formula, R a is C 1 -C 12 is an alkyl group, R b and R c are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or an organic group having 2 to 30 carbon atoms containing at least one aromatic ring, or a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted cycloalkyl group having 3 to 12 carbon atoms. A composition comprising at least two anisotropic compounds represented by the formula: wherein in a first anisotropic compound, ring F is represented by formula (IIa), and in a second anisotropic compound, ring F is represented by formula (IIb) or (IIc).

2. Rings C and D are each independently phenyl, cyclohexyl, [C10] The composition of claim 1 , selected from the group consisting of:

3. The composition according to claim 1 or 2, wherein n is an integer between 0 and 12.

4. The composition of claim 3, wherein n is an integer between 4 and 8.

5. The composition according to any one of claims 1 to 4, wherein in the group represented by formula (III), one or more carbon atoms are replaced by -O-.

6. R 1 , R 2 and R 3 are each independently hydrogen, lower alkyl, lower alkenyl, lower alkoxy, lower alkenyloxy, -F and -CF 3 The composition according to any one of claims 1 to 5, selected from the group consisting of:

7. R 1, R 2 and R 3 are each independently hydrogen, methyl, methoxy, -F, -C-(CH 3 ) 3 and -CF 3 The composition of claim 6, selected from the group consisting of:

8. The composition of any one of claims 1 to 7, wherein Ring E is phenyl.

9. The composition of any one of claims 1 to 8, wherein Z is selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

10. The composition according to any one of claims 1 to 9, wherein PG represents an acrylate or methacrylate group.

11. The composition according to any one of claims 1 to 10, wherein the anisotropic compound is in crosslinked or polymerized form.

12. An LCP network comprising the composition of any one of claims 1 to 11.

13. Use of a composition according to any one of claims 1 to 11 or an LCP network according to claim 12 in the manufacture of an optical or electro-optical device.

14. An optical or electro-optical device comprising a composition according to any one of claims 1 to 11 or an LCP network according to claim 12.

Citation Information

Patent Citations

  • Polymerizable compound, polymerizable composition, polymer, and optically anisotropic body

    US20160002374A1

  • Polymerizable compound, polymerizable composition, polymer, and optically anisotropic material

    WO2012147904A1

  • Polymerizable compound, polymerizable composition, polymer, and optically anisotropic body

    WO2014126113A1

  • Polymerizable composition and optically anisotropic body using same

    WO2016114252A1

  • Polymerizable composition and optically anisotropic body

    WO2016114255A1