The method addresses the challenge of attaching silicon timepiece components to a wafer without compromising the functional outer profile by using an SOI wafer structure and etching techniques to form anchors and bridges, enabling backside processing and decoration, thus enhancing manufacturing flexibility and integrity.
Patent Information
- Application Number
- JP2023090623
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-26
- Filing Date
- 2023-06-01
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-06-01
AI Technical Summary
Existing methods for manufacturing silicon timepiece components face challenges in attaching components to a wafer without compromising the functional outer profile, particularly when the backside needs processing or decoration, and are limited by the complexity of epitaxial growth and compatibility with commercially available substrates.
A method involving an SOI wafer with a silicon device layer, silicon oxide bonding layer, and silicon handle layer, using DRIE and wet etching to form anchors and bridges that allow components to be attached to the wafer while leaving the backside free for processing, with optional decoration through CVD or PVD.
Enables the manufacturing of silicon timepiece components with a functional outer profile by allowing access to the backside for manipulation and decoration, while maintaining structural integrity and avoiding interference with the outer contour.
Smart Images

Figure 0007564291000001 
Figure 0007564291000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a silicon timepiece component, in particular a silicon timepiece component having a functional outer profile. [Background technology]
[0002] Silicon timepiece components are typically manufactured by deep reactive ion etching (also known as DRIE) on a wafer made of silicon-based material. This wafer can be a silicon wafer that is etched through its entire thickness (see, for example, European patent applications EP1722281, EP2145857 and EP3181938), or a silicon-on-insulator (SOI) substrate with a top and bottom silicon layer connected by an intermediate silicon oxide layer, on which the etching is performed (see, for example, International patent applications WO2019 / 180177 and WO2019 / 180596). Silicon-on-insulator substrates have the advantage over a single silicon wafer of a rigid support (a bottom silicon layer that is thicker than the top silicon layer) for ease of handling and holding, and a barrier layer (an intermediate silicon oxide layer) to stop the etching.
[0003] Regardless of the type of wafer used, several components are etched simultaneously in the same wafer, leaving attachments or bridges left during etching that keep the components attached to the wafer for other manufacturing steps, and then releasing the components from the wafer by breaking or removing these attachments.
[0004] Such attachments, connecting the periphery of each component to the wafer, can be problematic, especially when the periphery of the component is a functional surface whose function must not be impaired by attachment residues, or when the outer surface of the component must have a particularly high appearance of integrity, such as in the case of needles. Also, in some cases, especially in components with fine teeth, there is not enough free space on the outer functional surface to provide a sufficiently strong attachment.
[0005] International patent application WO2019 / 166922 proposes a method for producing a balance spring in which a silicon substrate carrying a silicon oxide layer is provided, through-holes are formed in the silicon oxide layer, and a silicon layer is epitaxially grown on the silicon oxide layer. The silicon layer fills the through-holes to form attachments or material bridges, and the balance spring is etched in the silicon layer. The silicon oxide layer is removed, leaving the balance spring attached to the silicon substrate via the attachments. The balance spring is subjected to a heat treatment, and finally the balance spring is removed from the silicon substrate.
[0006] With such a method, the balance spring remains attached to the substrate after etching, not between the outer surface of the outermost turn and the silicon etched layer, as is typically the case, but by an attachment that extends out of the plane of the balance spring. However, this method does not allow the use of commercially available silicon-on-insulator substrates, and the epitaxial growth of the silicon layer from which the balance spring is formed is complicated to manipulate.
[0007] The international patent application WO2019 / 166922 is intended to overcome this problem and proposes a method for manufacturing a silicon timepiece component from an SOI wafer, in which the component is attached to an anchor inside the component's contour. This attachment therefore does not interfere with the functional outer contour of the component. However, this method does not allow processing on the back side of the component, especially in the case of components that require surface treatment or decoration. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention solves the above-mentioned problems by providing an approach that allows components to continue to be attached to the wafer, including components that do not allow for attachment to an outer contour, while leaving the back side free for processing and / or decoration.
[0009] To this end, the invention relates to a method for manufacturing a silicon timepiece component, a) providing a wafer, which is an SOI wafer, comprising, in order, a silicon "device" layer, a silicon oxide bonding layer, and a silicon "handle" layer; b) growing a silicon oxide layer on the face of the wafer; c) etching the silicon oxide layer at the surface of the wafer (etch mask) and etching the "device" layer by DRIE to define the timepiece components, inner anchor elements and material bridges connecting the anchor elements to the inner walls of the timepiece components in non-critical inner contour areas; d) etching the silicon oxide layer at the backside of the wafer (etching mask) and etching the "handle" layer by DRIE to define at least one narrow bridge and at least one anchor backside integral with the at least one narrow bridge and connected to the anchor element of the "device" layer by the silicon oxide bonding layer bonding the "device" layer and the "handle" layer; e) releasing said timepiece components by wet etching; The timepiece component is held on the wafer via the material bridges by the anchor elements, the silicon oxide bonding layer remaining only where both the "device" layer and the "handle" layer have not been etched away by the wet etch, and the entire timepiece component rests on the back side of the at least one anchor which is connected to the at least one narrow bridge, which is itself connected to the "handle" layer.
[0010] Another advantageous alternative embodiment of the invention has the following features: the inner wall of the timepiece component is the wall of a hole adapted to receive a shaft inside the component, or the wall of an opening inside the timepiece component. the silicon oxide bonding layer is partially present between the anchor element and the anchor backside at the end of step e). The narrow bridge and the material bridge do not overlap. - In step d), during DRIE of the "handle" layer, an integrated shadow mask is further formed, which creates a deliberate and intentional pattern of openings on the back surface, said openings allowing elaborate decoration by CVD or PVD. the method comprises a step f) of wafer finishing on the front and / or back surface of the timepiece component, said step f) consisting, for example, of depositing a layer, patterning and / or decorating. said timepiece component being a wheel, a cam, a hand, a lever, a snail, an index or an apex;
[0011] The invention further relates to a timepiece component obtainable by carrying out the method for manufacturing a timepiece component according to the invention.
[0012] It can thus be seen that the method makes it possible to access the back side of the wafer-mounted timepiece components so that it can be processed and / or decorated.
[0013] Other characteristics and advantages of the invention will appear clearly on reading the following detailed description, given by way of example with reference to the attached drawings, in which: [Brief description of the drawings]
[0014] [Figure 1] 1a and 1b show a perspective view of a silicon component integrated with the "device" layer and a perspective view of the "handle" layer, respectively. [Diagram 2] 2a and 2b show top and bottom perspective views, respectively, of a silicon component formed in a SOI wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention relates to a method for manufacturing a silicon timepiece component, in particular a silicon timepiece component having a functional outer profile.
[0016] A functional outer profile may be understood to mean a timepiece component whose outer periphery forms a functional surface adapted to cooperate with other parts and / or timepiece components.
[0017] The use of silicon-based materials for manufacturing timepiece components has the advantages of being accurate using existing etching methods, having good mechanical and chemical properties, and in particular being little or not affected by magnetic fields.
[0018] Preferably, the silicon-based material used can be monocrystalline silicon, regardless of its crystal orientation. Of course, other silicon-based compounds or other materials such as glasses, ceramics, cermets, metals or metal alloys can also be considered. For the sake of simplicity, in the following, silicon-based materials will be described.
[0019] As mentioned above, the present invention relates to a method for manufacturing a silicon timepiece component 1. The method of the present invention can also be used to manufacture other timepiece components such as gears, escape wheels, levers, snails, etc. It is also conceivable to use such a method of the present invention for the manufacture of hands, indexes or apexes, which require the highest possible integrity of the external surface finish.
[0020] According to the invention, the method comprises a first step a) which involves preparing an SOI wafer 10, as shown in Figure 2, i.e. a wafer with two silicon layers 11 and 12 bonded together by a silicon oxide layer 13. Each of these three layers has one or more specific roles.
[0021] The top silicon layer 11 (whose primary orientation can be changed) formed in a single crystal silicon wafer is called the "device" layer and typically has a thickness of 100-200 μm, which determines the final thickness of the manufactured component in a watch (e.g. wristwatch, pocket watch).
[0022] The bottom silicon layer 12 is called the "handle" layer and essentially acts as a mechanical support, allowing the method to be carried out on a sufficiently rigid assembly (such rigidity is not assured at the reduced thickness of the "device"). The bottom silicon layer 12 is also formed by a single crystal silicon wafer, typically of a similar orientation as the "device" layer.
[0023] The oxide layer 13 is used to intimately bond the two silicon layers 11 and 12 together and also serves as a barrier layer in subsequent operations.
[0024] The subsequent step b) involves growing a silicon oxide layer on the surface of the wafer or wafers 10 by exposing the wafer or wafers to a high temperature oxidizing atmosphere. This silicon oxide layer depends on the thickness of the "device" to be patterned, which is typically between 1 and 4 μm. Of course, other techniques can be used to form the etch mask, a photoresist layer may be sufficient, as in the next step c), and if an oxide is used it can be deposited rather than grown.
[0025] Step c) of the method makes it possible to define, for example in a positive photoresist, a pattern that is intended to be subsequently formed in the silicon wafer 10. This step c) comprises the following operations: - Deposit the photoresist in a very thin layer, typically 1-2 μm thick, for example by spin coating. After drying, a light source is used to expose the photoresist, which has photolithographic properties, through a photolithographic mask (a light-transmitting plate coated with a chrome layer representing the desired pattern). - In the specific case of positive photoresist, a solvent is used to remove the exposed areas of the photoresist to expose the oxide layer, where the areas still covered by photoresist form areas that should not be etched in a subsequent deep reactive ion etching process (also known as "DRIE") on silicon.
[0026] Thus, in step c) the exposed areas or, conversely, the areas covered with photoresist are utilized. A first etching process makes it possible to transfer the pattern formed in the photoresist in the previous step to the pre-grown silicon oxide. The silicon oxide is then patterned by a dry plasma etching which is also directional and reproduces, from the point of view of reproducibility of the manufacturing process, the quality of the sidewalls of the photoresist used as a mask for this operation.
[0027] Once the silicon oxide is etched in the open areas of the photoresist, the silicon surface of the top layer 11 is exposed and ready for DRIE. The photoresist may or may not be preserved, depending on whether the photoresist is used as an additional mask during DRIE.
[0028] The exposed silicon that is not protected by silicon oxide is etched in a direction perpendicular to the wafer surface (Bosch® Anisotropic DRIE). The pattern that is first formed in the photoresist and then in the silicon oxide is "projected" into the thickness of the "device" layer 11.
[0029] The etching stops when it reaches the silicon oxide layer 13 that bonds the two silicon layers 11 and 12. Notably, just like the example of silicon oxide that acts as a mask in the Bosch® process and is resistant to the etching process itself, the buried oxide layer 13 of the same nature is also resistant.
[0030] In this way, the silicon “device” layer 11 is patterned throughout its thickness with a predetermined pattern representative of the component to be fabricated, where this pattern, i.e., cam 1 in the illustrated example, is exposed by the DRIE.
[0031] The components remain integral with the "handle" layer 12 to which they are bonded through an embedded silicon oxide layer 13. In this step c), parts of the upper silicon layer 2 are etched to form anchor elements 7 inside the timepiece component and also to form material bridges 8 connecting said anchor elements 7 to the inner wall of the timepiece component 1 in non-critical areas of the inner wall of the timepiece component.
[0032] In the example shown, the inner wall of the timepiece component is the wall of a hole configured to receive the shaft. The hole has a shape such that it does not interfere with the arbor with which the rest of the attachment interfaces with the silicon plate. The inner wall can be that of another opening inside the component, such as in the case of a skeletonized case.
[0033] Of course, the method is not limited to etching by DRIE in step c) By way of example, the etching in step c) can equally be achieved by chemical etching for the same silicon-based materials.
[0034] In step c), multiple cams can be formed on the same wafer.
[0035] In step d), a second photolithography operation similar to the first photolithography operation performed in step c) is performed on the back side of the wafer 10 (i.e. the side of the "handle" layer 12). For this, the wafer 10 is turned over and a photoresist is deposited on it and exposed through a mask. During this second photolithography operation, at least one narrow bridge 9 is formed through the back side of the timepiece component and also an anchor backside 9' is formed integral with said at least one narrow bridge 9. This anchor backside 9' is connected to the anchor element 7 of the "device" layer by a silicon oxide layer that connects the "device" layer and the "handle" layer.
[0036] According to the invention, during DRIE of the "handle" layer in step d), an integrated shadow mask is also formed to create a deliberate and intentional pattern of openings on the backside, which openings make it possible to create complex decorations by CVD or PVD during a subsequent step.
[0037] The exposed areas of photoresist are then removed with a solvent to expose the previously formed oxide layer which acts as a mask for a deep dry etch such as DRIE, thereby exposing the at least one narrow bridge 9, anchor backside 9' and shadow mask.
[0038] In step e), the various silicon oxide layers are etched by a wet etching process using a hydrofluoric acid based solution or by hydrofluoric acid in the gas phase in order to completely release the components.Preferably, the formed cam 1 is held on the anchor element via a material bridge 8, the entire cam 1 resting on the anchor backside which is connected to said at least one narrow bridge, which itself is connected to a frame formed in the "handle" layer.
[0039] In step f), which is an optional step of the method, various surface finishing operations are performed on the released workpiece, still held by the attachment. Operations can thus be performed on the front, back and / or side of the timepiece component while it is still held on the wafer. This finishing step can involve depositing layers, patterning or decorating the different faces of the timepiece component. These operations can be of a functional nature (strengthening, tribological, etc.) or aesthetic nature (coloring, patterning), by PVD or CVD.
[0040] In this step, the pattern developed in step d) through a shadow mask is also decorated by CVD or PVD.
[0041] In this way, a cam 1 is obtained as shown in FIGS. 1a and 1b, which preferably, according to the invention, has a silicon-based core and a silicon oxide-based coating.
[0042] Advantageously, according to the invention, a timepiece component 1 having a functional outer profile can therefore be produced without complexity.
[0043] Finally, the method may also include a step h) of separating the timepiece component 1 from the wafer 10 by separating it from its anchoring elements 8 .
[0044] Naturally, the invention is not limited to the example shown, ie the manufacture of a cam, but is susceptible to various alternatives and variations which will be apparent to those skilled in the art. [Explanation of symbols]
[0045] 1 Timing Components 7 Anchor Elements 8 Material Bridge 9 Narrow Bridge 9' Anchor back side 10 Wafers 11 "Device" layer 12 "Handle" layer 13 Silicon oxide layer
Claims
1. A method for manufacturing a silicon timepiece component (1), comprising the steps of: a) providing a wafer (10) which is an SOI wafer comprising, in order, a silicon "device" layer (11), a silicon oxide bonding layer (13), and a silicon "handle" layer (12); b) growing a silicon oxide layer on at least the front and back surfaces of said wafer (10); c) etching the silicon oxide layer at the surface of the wafer (10) and etching the "device" layer (11) by DRIE to form the timepiece component (1), the inner anchor elements (7) and material bridges (8) connecting the anchor elements to the inner wall of the timepiece component in non-critical areas of said inner wall; d) etching the silicon oxide layer at the back side of the wafer (10) and etching the "handle" layer (12) by DRIE to form at least one narrow bridge (9) and at least one anchor backside (9') integral with the at least one narrow bridge (9) and connected to the anchor element (7) of the "device" layer by the silicon oxide bonding layer (13) bonding the "device" layer and the "handle" layer; e) releasing said timepiece component (1) by wet etching, said timepiece component (1) being held on said wafer (10) via said material bridge (8) by said anchoring elements (7); the silicon oxide bonding layer remains only where both the "device" layer and the "handle" layer have not been etched or removed by the wet etch; the entirety of the timepiece component rests on the underside (9') of the at least one anchor connected to the at least one narrow bridge (9); The narrow bridge (9) itself is connected to the "handle" layer to allow access to all sides of the timepiece component. A method comprising:
2. The inner wall of the timepiece component (1) is the wall of a hole designed to receive a shaft inside the component or the wall of an opening inside the timepiece component.
2. The method of claim 1 .
3. The silicon oxide bonding layer (13) is partially present between the anchor element (7) and the anchor backside (9') at the end of step e).
2. The method of claim 1 .
4. The narrow bridge (9) and the material bridge (8) do not overlap.
2. The method of claim 1 .
5. In step d), during DRIE of the "handle" layer, further forming an integrated shadow mask, thereby creating a deliberate and intentional pattern of openings in the back surface; The openings allow for elaborate decoration by deposition 2. The method of claim 1 .
6. f) a wafer finish on the front, back and / or side of the timepiece component (1), Step f) includes depositing a layer, patterning and / or decorating.
2. The method of claim 1 .
7. The timepiece component is a wheel, a cam, a hand, a lever, a snail, an index, or an apex.
2. The method of claim 1 .
8. Obtained by carrying out the method according to claim 1 A component (1) for a timepiece, characterized in that
Citation Information
Patent Citations
Manufacturing method for timepiece component
JP2017044533A
Multistage micromechanical timepiece and method for making same
US20200050150A1