Piezoelectric device, liquid ejection head, liquid ejection apparatus, and method for manufacturing piezoelectric device
By employing a substrate with recesses and varying crystal orientations in the piezoelectric layer, the piezoelectric device addresses heat-related cracking issues, improving durability and reliability.
Patent Information
- Application Number
- JP2020182234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Piezoelectric layers in piezoelectric devices, such as inkjet recording heads, are prone to cracks and damage due to heat generation caused by bending deformation, which worsens with improved performance, leading to potential failure.
The piezoelectric device incorporates a substrate with recesses and a diaphragm, featuring a piezoelectric actuator with a first electrode, piezoelectric layer, and second electrode, where the piezoelectric layer has different crystal orientations and thicknesses in specific regions to manage heat generation and deformation.
This configuration effectively suppresses heat generation and deformation, reducing the risk of cracks and enhancing the durability and reliability of the piezoelectric actuator.
Smart Images

Figure 0007564504000001 
Figure 0007564504000002 
Figure 0007564504000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric device including a vibration plate and a piezoelectric actuator having a first electrode, a piezoelectric layer, and a second electrode, a liquid ejecting head, a liquid ejecting apparatus, and a method for manufacturing a piezoelectric device. [Background technology]
[0002] A representative example of a liquid jet head, which is a piezoelectric device, is an ink jet recording head that jets ink droplets. An ink jet recording head is known that includes, for example, a flow path forming substrate in which a pressure chamber communicating with a nozzle is formed, and a piezoelectric actuator provided on one side of the flow path forming substrate via a vibration plate, and jets ink droplets from the nozzle by causing a pressure change in the ink in the pressure chamber with the piezoelectric actuator.
[0003] Also, a piezoelectric actuator is known that includes a first electrode formed on a vibration plate, a piezoelectric layer formed on the first electrode from a piezoelectric material having electromechanical conversion properties, and a second electrode provided on the piezoelectric layer. In a piezoelectric actuator of this configuration, there is a risk that cracks or burnout may occur in the piezoelectric layer due to bending deformation of the piezoelectric layer. In order to prevent the occurrence of such defects, various configurations of piezoelectric actuators (piezoelectric elements) have been proposed (for example, see Patent Document 1).
[0004] Patent document 1 describes that the piezoelectric element extends outside the opening of the pressure chamber cavity, and the width of the first electrode layer constituting the piezoelectric element is narrower outside the pressure chamber cavity than in the area corresponding to the pressure chamber cavity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-171809 A Summary of the Invention [Problem to be solved by the invention]
[0006] In a configuration in which the piezoelectric actuator extends to the outside of the pressure chamber, there is a problem that cracks may occur in the piezoelectric layer as described above, and furthermore, since the piezoelectric layer extending to the outside of the pressure chamber does not flex and deform when a voltage is applied, heat is generated by the current that flows at that time. As the performance of the piezoelectric layer improves, the heat generated by the piezoelectric layer tends to increase, and there is a risk that the piezoelectric actuator may be damaged due to this heat generation.
[0007] It should be noted that such problems are not limited to liquid ejection heads such as ink jet recording heads that eject ink, but also exist in other piezoelectric devices. [Means for solving the problem]
[0008] One aspect of the present invention that solves the above problem is a piezoelectric device comprising a substrate having a plurality of recesses formed therein, a vibration plate provided on one side of the substrate, a first electrode stacked in a first direction on the side of the vibration plate opposite the substrate, a piezoelectric layer, and a piezoelectric actuator having a second electrode, wherein when, of two regions of the second electrode in a second direction intersecting the first direction, one region farther from an end of the second electrode is defined as a first region and one region closer to the end of the second electrode is defined as a second region, the piezoelectric layer in the first region has a (100) plane preferred orientation and the (100) plane orientation rate of the piezoelectric layer in the second region is lower than the (100) plane orientation rate of the piezoelectric layer in the first region.
[0009] Another aspect of the present invention is a liquid jet head comprising a substrate having a plurality of recesses formed therein, a vibration plate provided on one side of the substrate, a first electrode stacked in a first direction on the side of the vibration plate opposite the substrate, a piezoelectric layer, and a piezoelectric actuator having a second electrode, wherein when, of two regions of the second electrode in a second direction intersecting the first direction, one region farther from an end of the second electrode is defined as a first region and one region closer to the end of the second electrode is defined as a second region, the piezoelectric layer in the first region has a (100) plane preferred orientation and the (100) plane orientation rate of the piezoelectric layer in the second region is lower than the (100) plane orientation rate of the piezoelectric layer in the first region.
[0010] Another aspect of the present invention is a liquid ejecting apparatus including the above-mentioned liquid ejecting head.
[0011] Yet another aspect of the present invention is a piezoelectric actuator including a substrate having a plurality of recesses formed therein, a vibration plate provided on one side of the substrate, a first electrode laminated in a first direction on the side of the vibration plate opposite the substrate, a piezoelectric layer, and a second electrode, and wherein one of two regions of the second electrode in a second direction intersecting the first direction that is far from an end of the second electrode is provided with a piezoelectric layer. region a region close to an end of the second electrode is defined as a first region, the piezoelectric layer in the first region has a (100) plane preferential orientation, and a (100) plane orientation rate of the piezoelectric layer in the second region is lower than the (100) plane orientation rate of the piezoelectric layer in the first region, the method for manufacturing a piezoelectric device comprising the steps of: laminating the first electrode, the piezoelectric layer, and the second electrode on a surface of the vibration plate provided on the substrate to form the piezoelectric actuator; forming an orientation control layer for controlling the crystal orientation of the piezoelectric layer; and forming the orientation control layer, the orientation control layer is formed to different thicknesses in the first region and the second region. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is an exploded perspective view of the recording head according to the first embodiment. [Diagram 2] FIG. 2 is a plan view of the recording head according to the first embodiment. [Diagram 3] 1 is a cross-sectional view of a recording head according to a first embodiment. [Figure 4] 2 is a cross-sectional view of a main part of a recording head according to the first embodiment. FIG. [Diagram 5] 1 is a cross-sectional view of a recording head according to a first embodiment. [Figure 6] 5 is a cross-sectional view showing a main part of a modified example of the recording head according to the first embodiment. FIG. [Figure 7] 5 is a cross-sectional view showing a main part of a modified example of the recording head according to the first embodiment. FIG. [Figure 8] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 9] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 10] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 11] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 12] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 13] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 14] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 15] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 16] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 17] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 18] 5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 19]5A to 5C are cross-sectional views illustrating a method for manufacturing the recording head according to the first embodiment. [Figure 20] 5A to 5C are cross-sectional views showing another example of the method for manufacturing the recording head according to the first embodiment. [Figure 21] FIG. 11 is a cross-sectional view of a main part of a recording head according to a second embodiment. [Figure 22] FIG. 11 is a cross-sectional view of a main part of a recording head according to a second embodiment. [Figure 23] FIG. 1 is a diagram showing a schematic configuration of a recording apparatus according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below based on an embodiment. However, the following description is only one aspect of the present invention, and the configuration of the present invention can be modified as desired within the scope of the invention. In each drawing, the same members are given the same reference numerals, and duplicated descriptions will be omitted.
[0014] In each figure, X, Y, and Z represent three spatial axes that are orthogonal to each other. In this specification, the directions along these axes are referred to as the X direction, Y direction, and Z direction. In each figure, the direction indicated by the arrow is the positive (+) direction, and the opposite direction to the arrow is the negative (-) direction. The Z direction indicates the vertical direction, with the +Z direction pointing vertically downward and the -Z direction pointing vertically upward. Furthermore, the three spatial axes X, Y, and Z, which are not limited to positive and negative directions, will be described as the X axis, Y axis, and Z axis.
[0015] (Embodiment 1) Fig. 1 is an exploded perspective view of an ink jet recording head which is an example of a liquid jet head according to a first embodiment of the present invention. Fig. 2 is a plan view of the recording head. Fig. 3 is a cross-sectional view taken along line AA' in Fig. 2, Fig. 4 is an enlarged view of a piezoelectric actuator portion in Fig. 3, and Fig. 5 is a cross-sectional view taken along line BB' in Fig. 2, showing an enlarged view of the piezoelectric actuator portion.
[0016] As shown in the figure, an ink jet recording head (hereinafter also simply referred to as a recording head) 1, which is an example of a liquid jet head of this embodiment, jets ink droplets in a first direction, that is, the Z axis direction, more specifically, in the +Z direction.
[0017] The inkjet recording head 1 includes a flow path forming substrate 10 as an example of a substrate. The flow path forming substrate 10 is made of, for example, a silicon substrate, a glass substrate, an SOI substrate, various ceramic substrates, etc. The flow path forming substrate 10 may be a substrate having a (100) plane preferential orientation, or a substrate having a (110) plane preferential orientation.
[0018] In the flow path forming substrate 10, a plurality of pressure chambers 12 are arranged in two rows in the X-axis direction, which is a second direction intersecting with the Z-axis direction, which is a first direction. That is, the plurality of pressure chambers 12 constituting each row are arranged along the Y-axis direction, which is a third direction intersecting with the X-axis direction.
[0019] The multiple pressure chambers 12 constituting each row are arranged on a straight line along the Y axis direction so that they are positioned at the same position in the X axis direction. Pressure chambers 12 adjacent to each other in the Y axis direction are partitioned by partition walls 11. Of course, the arrangement of the pressure chambers 12 is not particularly limited. For example, the arrangement of the multiple pressure chambers 12 lined up in the Y axis direction may be a so-called staggered arrangement in which every other pressure chamber 12 is shifted in the X axis direction.
[0020] Furthermore, the pressure chamber 12 in this embodiment is formed, for example, in a rectangular shape, with the length in the X-axis direction being longer than the length in the Y-axis direction when viewed in a plan view from the +Z direction. Of course, the shape of the pressure chamber 12 when viewed in a plan view from the +Z direction is not particularly limited, and may be a parallelogram, polygon, circle, oval, or the like. Note that the oval shape referred to here refers to a shape that is based on a rectangular shape and has semicircular ends at both longitudinal ends, and includes a rounded rectangular shape, an elliptical shape, an egg shape, and the like.
[0021] On the +Z direction side of the flow passage forming substrate 10, a communication plate 15, a nozzle plate 20, and a compliance substrate 45 are laminated in this order.
[0022] The communicating plate 15 is provided with nozzle communicating passages 16 that communicate between the pressure chambers 12 and the nozzles 21. The communicating plate 15 is also provided with a first manifold portion 17 and a second manifold portion 18 that constitute a part of a manifold 100 that serves as a common liquid chamber to which the multiple pressure chambers 12 communicate. The first manifold portion 17 is provided so as to penetrate the communicating plate 15 in the Z-axis direction. The second manifold portion 18 is provided so as to open on the surface on the +Z direction side, without penetrating the communicating plate 15 in the Z-axis direction.
[0023] Furthermore, in the communicating plate 15, a supply communication passage 19 that communicates with one end of the pressure chamber 12 in the X-axis direction is provided independently for each pressure chamber 12. The supply communication passage 19 communicates between the second manifold portion 18 and each pressure chamber 12, and supplies ink in the manifold 100 to each pressure chamber 12.
[0024] The communicating plate 15 may be a silicon substrate, a glass substrate, an SOI substrate, various ceramic substrates, a metal substrate, or the like. Examples of metal substrates include a stainless steel substrate. The communicating plate 15 is preferably made of a material having a thermal expansion coefficient substantially the same as that of the flow path forming substrate 10. This makes it possible to suppress warping of the flow path forming substrate 10 and the communicating plate 15 caused by the difference in thermal expansion coefficient when the temperatures of the flow path forming substrate 10 and the communicating plate 15 change.
[0025] The nozzle plate 20 is provided on the side of the communication plate 15 opposite to the flow path forming substrate 10, i.e., on the +Z direction side. Nozzles 21 communicating with each pressure chamber 12 via nozzle communication paths 16 are formed in the nozzle plate 20.
[0026] In this embodiment, the multiple nozzles 21 are arranged in a line along the Y-axis direction. The nozzle plate 20 is provided with two nozzle rows in the X-axis direction, each row having the multiple nozzles 21 arranged therein. That is, the multiple nozzles 21 in each row are arranged so that their positions in the X-axis direction are the same. The arrangement of the nozzles 21 is not particularly limited. For example, the nozzles 21 arranged in a line in the Y-axis direction may be arranged at positions shifted in the X-axis direction every other nozzle 21.
[0027] The material of the nozzle plate 20 is not particularly limited, and may be, for example, a silicon substrate, a glass substrate, an SOI substrate, various ceramic substrates, or a metal substrate. Examples of metal plates include stainless steel substrates. Furthermore, organic materials such as polyimide resins may also be used as the material of the nozzle plate 20. However, it is preferable that the nozzle plate 20 is made of a material having a thermal expansion coefficient substantially equal to that of the communication plate 15. This makes it possible to suppress warping of the nozzle plate 20 and the communication plate 15 caused by the difference in thermal expansion coefficient when the temperature of the nozzle plate 20 and the communication plate 15 changes.
[0028] The compliance substrate 45 is provided together with the nozzle plate 20 on the side of the communication plate 15 opposite to the flow passage forming substrate 10, i.e., on the surface on the +Z direction side. The compliance substrate 45 is provided around the nozzle plate 20 and seals the openings of the first manifold portion 17 and the second manifold portion 18 provided on the communication plate 15. In this embodiment, the compliance substrate 45 includes a sealing film 46 made of a flexible thin film and a fixed substrate 47 made of a hard material such as metal. The region of the fixed substrate 47 facing the manifold 100 is an opening 48 that is completely removed in the thickness direction. Therefore, one surface of the manifold 100 is a compliance portion 49 sealed only by the sealing film 46 having flexibility.
[0029] On the other hand, on the side of the flow path forming substrate 10 opposite to the nozzle plate 20 etc., i.e., on the surface on the -Z direction side, there are provided a vibration plate 50 and a piezoelectric actuator 300 that flexes and deforms the vibration plate 50 to cause a pressure change in the ink in the pressure chamber 12, as will be described in detail later. Note that Fig. 3 is a diagram for explaining the overall configuration of the recording head 1, and the configuration of the piezoelectric actuator 300 is shown in a simplified manner.
[0030] A protective substrate 30 having approximately the same size as the flow path forming substrate 10 is further bonded to the surface of the flow path forming substrate 10 on the -Z direction side by an adhesive or the like. The protective substrate 30 has a holding portion 31 which is a space for protecting the piezoelectric actuators 300. The holding portion 31 is provided independently for each row of the piezoelectric actuators 300 arranged side by side in the Y axis direction, and two holding portions 31 are formed side by side in the X axis direction. In addition, the protective substrate 30 is provided with a through hole 32 penetrating in the Z axis direction between the two holding portions 31 arranged side by side in the X axis direction.
[0031] In addition, a case member 40 is fixed onto the protective substrate 30. The case member 40 defines, together with the flow path forming substrate 10, a manifold 100 that communicates with the multiple pressure chambers 12. The case member 40 has approximately the same shape as the above-mentioned communicating plate 15 in a plan view, and is joined to the protective substrate 30 and also to the above-mentioned communicating plate 15.
[0032] Such a case member 40 has an accommodation section 41 on the protective substrate 30 side, which is a space deep enough to accommodate the flow path forming substrate 10 and the protective substrate 30. This accommodation section 41 has an opening area larger than the surface of the protective substrate 30 joined to the flow path forming substrate 10. Then, with the flow path forming substrate 10 and the protective substrate 30 accommodated in the accommodation section 41, the opening surface of the accommodation section 41 on the nozzle plate 20 side is sealed by a communication plate 15.
[0033] Additionally, third manifold portions 42 are defined on both outer sides of the accommodation portion 41 in the X-axis direction in the case member 40. The manifold 100 of this embodiment is configured by the first manifold portion 17 and the second manifold portion 18 provided in the communication plate 15, and the third manifold portion 42. The manifold 100 is provided continuously along the Y-axis direction, and the supply communication passages 19 that communicate between each pressure chamber 12 and the manifold 100 are arranged side by side in the Y-axis direction.
[0034] Moreover, the case member 40 is provided with an inlet 44 that communicates with the manifolds 100 and supplies ink to each manifold 100. Furthermore, the case member 40 is provided with a connection port 43 that communicates with the through hole 32 of the protection substrate 30 and through which the wiring substrate 120 is inserted.
[0035] In the recording head 1 of this embodiment, ink is taken in from the inlet 44 connected to an external ink supply means (not shown), and the inside is filled with ink from the manifold 100 to the nozzles 21. Then, a voltage is applied to each piezoelectric actuator 300 corresponding to each pressure chamber 12 in accordance with a recording signal from the drive circuit 121. This causes the piezoelectric actuator 300 and the diaphragm 50 to bend and deform, increasing the pressure inside each pressure chamber 12, and ink droplets are ejected from each nozzle 21.
[0036] The following describes the configuration of the piezoelectric actuator 300 according to this embodiment. As described above, the piezoelectric actuator 300 is provided on the surface of the flow passage forming substrate 10 opposite to the nozzle plate 20, with the vibration plate 50 interposed therebetween.
[0037] 3 to 5, the vibration plate 50 is composed of an elastic film 51 made of silicon oxide provided on the flow path forming substrate 10 side, and an insulating film 52 made of zirconium oxide provided on the elastic film 51. The liquid flow paths such as the pressure chambers 12 are formed by anisotropically etching the flow path forming substrate 10 from the surface on the +Z direction side, and the surface on the -Z direction side of the liquid flow paths such as the pressure chambers 12 is composed of the elastic film 51.
[0038] The configuration of the diaphragm 50 is not particularly limited. The diaphragm 50 may be composed of, for example, either the elastic film 51 or the insulating film 52, or may include other films in addition to the elastic film 51 and the insulating film 52. Examples of materials for the other films include silicon, silicon nitride, and the like.
[0039] The piezoelectric actuator 300 is a pressure generating means that generates a pressure change in the ink in the pressure chamber 12, and is also called a piezoelectric element. This piezoelectric actuator 300 includes a first electrode 60, a piezoelectric layer 70, and a second electrode 80 that are sequentially stacked from the +Z direction side, which is the vibration plate 50 side, toward the -Z direction side. That is, the piezoelectric actuator 300 includes the first electrode 60, the piezoelectric layer 70, and the second electrode 80 that are sequentially stacked along the Z-axis direction, which is a first direction, relative to the vibration plate 50, toward the -Z direction side in this embodiment.
[0040] In the piezoelectric actuator 300, a portion where a piezoelectric strain occurs in the piezoelectric layer 70 when a voltage is applied between the first electrode 60 and the second electrode 80 is referred to as an active portion 310. In contrast, a portion where no piezoelectric strain occurs in the piezoelectric layer 70 is referred to as an inactive portion 320. That is, in the piezoelectric actuator 300, a portion where the piezoelectric layer 70 is sandwiched between the first electrode 60 and the second electrode 80 is the active portion 310, and a portion where the piezoelectric layer 70 is not sandwiched between the first electrode 60 and the second electrode is the inactive portion 320. In addition, when the piezoelectric actuator 300 is driven, a portion that actually displaces in the Z-axis direction is referred to as a flexible portion, and a portion that does not displace in the Z-axis direction is referred to as a non-flexible portion. That is, in the piezoelectric actuator 300, a portion facing the pressure chamber 12 in the Z-axis direction is a flexible portion, and a portion outside the pressure chamber 12 is a non-flexible portion.
[0041] In general, one of the electrodes of the active portions 310 is configured as an individual electrode independent for each active portion 310, and the other electrode is configured as a common electrode common to the multiple active portions 310. In this embodiment, the first electrode 60 constitutes the individual electrode, and the second electrode 80 constitutes the common electrode.
[0042] Specifically, the first electrode 60 is separated for each pressure chamber 12 to form an independent individual electrode for each active portion 310. The first electrode 60 is formed with a width narrower than the width of the pressure chamber 12 in the Y-axis direction. That is, in the Y-axis direction, the end of the first electrode 60 is located inside the region facing the pressure chamber 12.
[0043] Further, the +X direction end 60a and the -X direction end 60b of the first electrode 60 are each disposed outside the pressure chamber 12. As shown in Fig. 4, the +X direction end 60a of the first electrode 60 is disposed in a position more in the +X direction than the +X direction end 12a of the pressure chamber 12. The -X direction end 60b of the first electrode 60 is disposed in a position more in the -X direction than the -X direction end 12b of the pressure chamber 12.
[0044] The material of the first electrode 60 is not particularly limited, but may be, for example, a conductive material such as a metal such as iridium or platinum, or a conductive metal oxide such as indium tin oxide, abbreviated as ITO.
[0045] As shown in FIG. 2, the piezoelectric layer 70 is provided continuously in the Y-axis direction with a predetermined length in the X-axis direction. That is, the piezoelectric layer 70 is provided continuously in the arrangement direction of the pressure chambers 12 with a predetermined thickness. The thickness of the piezoelectric layer 70 is not particularly limited, but is formed to a thickness of about 1 to 4 μm. As shown in FIG. 4, the length of the piezoelectric layer 70 in the X-axis direction is longer than the length of the pressure chambers 12 in the X-axis direction, which is the longitudinal direction of the pressure chambers 12. Therefore, on both sides of the pressure chambers 12 in the X-axis direction, the piezoelectric layer 70 extends to the outside of the pressure chambers 12. In this way, the strength of the vibration plate 50 is improved by the piezoelectric layer 70 extending to the outside of the pressure chambers 12 in the X-axis direction. Therefore, when the active portion 310 is driven to displace the piezoelectric actuator 300, it is possible to suppress the occurrence of cracks and the like in the piezoelectric layer 70.
[0046] 4, the end 70a in the +X direction of the piezoelectric layer 70 is located outside the end 60a of the first electrode 60. That is, the end 60a in the +X direction of the first electrode 60 is covered by the piezoelectric layer 70. On the other hand, the end 70b in the -X direction of the piezoelectric layer 70 is located inside the end 60b of the first electrode 60, and the end 60b in the -X direction of the first electrode 60 is not covered by the piezoelectric layer 70.
[0047] 2 and 5, the piezoelectric layer 70 has grooves 71 that correspond to the partition walls 11 and are thinner than other regions. The grooves 71 in this embodiment are formed by completely removing the piezoelectric layer 70 in the Z-axis direction. That is, the piezoelectric layer 70 having a portion thinner than other regions includes the piezoelectric layer 70 being completely removed in the Z-axis direction. Of course, the piezoelectric layer 70 may be formed thinner on the bottom surface of the grooves 71 than other portions.
[0048] The length of the groove 71 in the Y-axis direction, i.e., the width of the groove 71, is equal to or greater than the width of the partition wall 11. In this embodiment, the width of the groove 71 is greater than the width of the partition wall 11.
[0049] Such groove portion 71 is formed to have a rectangular shape when viewed from the -Z direction side. Of course, the shape of groove portion 71 when viewed from the -Z direction side is not limited to a rectangular shape, and may be a polygonal shape having 5 or more sides, a circular shape, an elliptical shape, or the like.
[0050] By providing groove portion 71 in piezoelectric layer 70, the rigidity of the portion of vibration plate 50 facing the end of pressure chamber 12 in the Y-axis direction, i.e., the arm portion of vibration plate 50, is reduced, thereby allowing piezoelectric actuator 300 to be displaced more effectively.
[0051] The piezoelectric layer 70 may be a crystal film (perovskite type crystal) having a perovskite structure and made of a ferroelectric ceramic material exhibiting an electromechanical conversion function formed on the first electrode 60. The material of the piezoelectric layer 70 may be, for example, a ferroelectric piezoelectric material such as lead zirconate titanate (PZT) or a material to which a metal oxide such as niobium oxide, nickel oxide, or magnesium oxide is added. Specifically, lead titanate (PbTiO3), lead zirconate titanate (Pb(Zr,Ti)O3), lead zirconate (PbZrO3), lead lanthanum titanate ((Pb,La),TiO3), lead lanthanum zirconate titanate ((Pb,La)(Zr,Ti)O3), or magnesium zirconate titanate (Pb(Zr,Ti)(Mg,Nb)O3). In this embodiment, lead zirconate titanate (PZT) is used as the piezoelectric layer 70.
[0052] Furthermore, the material of the piezoelectric layer 70 is not limited to lead-based piezoelectric materials that contain lead, and lead-free piezoelectric materials that do not contain lead can also be used. Examples of lead-free piezoelectric materials include bismuth ferrate ((BiFeO3), abbreviated as "BFO"), barium titanate ((BaTiO3), abbreviated as "BT"), potassium sodium niobate ((K,Na)(NbO3), abbreviated as "KNN"), potassium sodium lithium niobate ((K,Na,Li)(NbO3)), potassium sodium lithium tantalate niobate ((K,Na,Li)(Nb,Ta)O3), bismuth potassium titanate ((Bi 1 / 2 K 1 / 2 )TiO3, abbreviated as "BKT"), sodium bismuth titanate ((Bi 1 / 2 Na 1 / 2 )TiO3, abbreviated as "BNT"), bismuth manganate (BiMnO3, abbreviated as "BM"), and complex oxides containing bismuth, potassium, titanium, and iron and having a perovskite structure (x[(Bi x K 1-x)TiO3]-(1-x)[BiFeO3], abbreviated as "BKT-BF"); complex oxides containing bismuth, iron, barium and titanium and having a perovskite structure ((1-x)[BiFeO3]-x[BaTiO3], abbreviated as "BFO-BT"); and those to which metals such as manganese, cobalt and chromium have been added ((1-x)[Bi(Fe 1-y M y )O3]-x[BaTiO3] (M is Mn, Co or Cr)).
[0053] As shown in Figs. 4 and 5, the second electrode 80 is provided on the -Z direction side of the piezoelectric layer 70, which is the opposite side to the first electrode 60, and constitutes a common electrode common to the multiple active sections 310. The second electrode 80 is provided continuously along the Y direction with a predetermined length along the X direction. The second electrode 80 is also provided on the inner surface of the groove 71, that is, on the side surface of the groove 71 of the piezoelectric layer 70 and on the insulating film 52 which is the bottom surface of the groove 71. Note that, with respect to the inside of the groove 71, the second electrode 80 may be provided only on a part of the inner surface of the groove 71, and may not be provided over the entire inner surface of the groove 71.
[0054] 4, the end 80a in the +X direction of the second electrode 80 is disposed so as to be outside the end 60a in the +X direction of the first electrode 60 covered with the piezoelectric layer 70. That is, the end 80a in the +X direction of the second electrode 80 is located outside the end 12a in the +X direction of the pressure chamber 12 and outside the end 60a of the first electrode 60. In this embodiment, the end 80a in the +X direction of the second electrode 80 substantially coincides with the end 70a of the piezoelectric layer 70. Therefore, the end in the +X direction of the active portion 310, i.e., the boundary between the active portion 310 and the inactive portion 320, is defined by the end 60a of the first electrode 60.
[0055] On the other hand, the -X direction end 80b of the second electrode 80 is disposed outside the -X direction end 12b of the pressure chamber 12, but inside the X-axis direction end 70b of the piezoelectric layer 70. As described above, the -X direction end 70b of the piezoelectric layer 70 is located inside the end 60b of the first electrode 60. Therefore, the -X direction end 80b of the second electrode 80 is located on the piezoelectric layer 70 inside the -X direction end 60b of the first electrode 60. Therefore, outside the -X direction end 80b of the second electrode 80, there is a portion where the surface of the piezoelectric layer 70 is exposed.
[0056] In this way, the -X direction end 80b of the second electrode 80 is positioned on the +X direction side of the -X direction ends of the piezoelectric layer 70 and the first electrode 60, and therefore the -X direction end of the active portion 310, i.e., the boundary between the active portion 310 and the inactive portion 320, is defined by the -X direction end 80b of the second electrode 80.
[0057] The material of the second electrode 80 is not particularly limited, but similar to the first electrode 60, for example, a conductive material such as a metal such as iridium or platinum, or a conductive metal oxide such as indium tin oxide is suitably used.
[0058] Further, outside the end 80b of the second electrode 80 in the -X direction, that is, on the further -X direction side of the end 80b of the second electrode 80, a wiring portion 85 is provided which is made of the same layer as the second electrode 80 but is electrically discontinuous with the second electrode 80. The wiring portion 85 is formed on the piezoelectric layer 70 and on the first electrode 60 which is extended in the -X direction beyond the piezoelectric layer 70, with a gap therebetween so as not to contact the end 80b of the second electrode 80 in the -X direction. This wiring portion 85 is provided independently for each active portion 310. That is, a plurality of wiring portions 85 are arranged at predetermined intervals along the Y-axis direction. The wiring portion 85 may be formed in a layer different from the second electrode 80, but is preferably formed in the same layer as the second electrode 80. This simplifies the manufacturing process of the wiring portion 85 and reduces costs.
[0059] Further, an individual lead electrode 91 and a common lead electrode 92, which is a common electrode for driving, are connected to the first electrode 60 and the second electrode 80 constituting the piezoelectric actuator 300, respectively. A flexible wiring board 120 is connected to the ends of the individual lead electrode 91 and the common lead electrode 92 opposite to the ends connected to the piezoelectric actuator 300. In this embodiment, the individual lead electrode 91 and the common lead electrode 92 are extended so as to be exposed in a through hole 32 formed in the protection substrate 30, and are electrically connected to the wiring board 120 within this through hole 32. A driving circuit 121 having a switching element for driving the piezoelectric actuator 300 is mounted on the wiring board 120.
[0060] In this embodiment, the individual lead electrode 91 and the common lead electrode 92 are made of the same layer, but are formed so as to be electrically discontinuous. This simplifies the manufacturing process and reduces costs compared to when the individual lead electrode 91 and the common lead electrode 92 are formed separately. Of course, the individual lead electrode 91 and the common lead electrode 92 may be formed in different layers.
[0061] The material of the individual lead electrode 91 and the common lead electrode 92 is not particularly limited as long as it is a material having electrical conductivity, and for example, gold (Au), platinum (Pt), aluminum (Al), copper (Cu), etc. can be used. In this embodiment, gold (Au) is used for the individual lead electrode 91 and the common lead electrode 92. In addition, the individual lead electrode 91 and the common lead electrode 92 may have an adhesion layer that improves adhesion with the first electrode 60, the second electrode 80, and the diaphragm 50.
[0062] The individual lead electrodes 91 are provided for each active portion 310, i.e., for each first electrode 60. The individual lead electrodes 91 are connected to the vicinity of the end portions 60b in the -X direction of the first electrodes 60 provided on the outer sides of the piezoelectric layers 70 via wiring portions 85, and are drawn out in the -X direction onto the flow path forming substrate 10, actually onto the vibration plate 50.
[0063] On the other hand, the common lead electrode 92 is drawn in the -X direction from above the second electrode 80 constituting the common electrode on the piezoelectric layer 70 onto the vibration plate 50 at both ends in the Y axis direction. The common lead electrode 92 also has an extension portion 93 extending along the Y axis direction in a region corresponding to the end 12b on the -X direction side of the pressure chamber 12. The common lead electrode 92 further includes an extension portion 94 extending along the Y axis direction in a region corresponding to the end 12a on the +X direction side of the pressure chamber 12. These extension portions 93, 94 are continuously provided over the Y axis direction for the multiple active portions 310. As described above, the common lead electrode 92 is drawn in the -X direction onto the vibration plate 50 at both ends in the Y axis direction.
[0064] The extension portions 93, 94 extend from the inside of the pressure chamber 12 to the outside of the pressure chamber 12. In this embodiment, the active portion 310 of the piezoelectric actuator 300 extends to the outside of the pressure chamber 12 at both ends of the pressure chamber 12 in the X-axis direction, and the extension portions 93, 94 extend on the active portions 310 to the outside of the pressure chamber 12.
[0065] In the piezoelectric actuator 300 according to this embodiment, when one of the two regions in the X-axis direction of the second electrode 80 that is farther from the end 80b of the second electrode 80 is defined as a first region S1 and the other region that is closer to the end 80b of the second electrode 80 is defined as a second region S2, the piezoelectric layer 70 in the first region S1 has a (100) plane preferred orientation, and the (100) plane orientation rate of the piezoelectric layer 70 in the second region S2 is lower than the (100) plane orientation rate of the piezoelectric layer 70 in the first region S1.
[0066] In other words, the piezoelectric layer 70 has a first orientation portion 75 in the first region S1 that has a (100) plane preferential orientation, and has a second orientation portion 76 in the second region S2 that has a lower (100) plane orientation rate than the first orientation portion 75.
[0067] Specifically, the first region S1 and the second region S2 are as follows: The first region S1 is a region located within a driving region where the vibration plate 50 contacts the pressure chamber 12, which is a recess. The second region S2 is a region located within a non-driving region where the vibration plate 50 does not contact the pressure chamber 12. In other words, the first region S1 is a region inside the pressure chamber 12, preferably near the center of the pressure chamber 12 in the X-axis direction, and the second region S2 is a region outside the end 12b of the pressure chamber 12 in the -X direction.
[0068] That is, the piezoelectric layer 70 has a first orientation section 75 with a (100) plane preferential orientation in a region facing the pressure chamber 12, and has a second orientation section 76 with a lower (100) plane orientation rate than the first orientation section 75 in a region outside the end 12b of the pressure chamber 12 in the -X direction. In this embodiment, the piezoelectric layer 70 is mainly composed of the first orientation section 75 with a (100) plane preferential orientation, and has the second orientation section 76 with a lower (100) plane orientation rate than the first orientation section 75 in a part of the region outside the pressure chamber 12.
[0069] In this specification, the term "preferentially oriented" refers to 50% or more, preferably 80% or more, of the crystals being oriented in a specific crystal plane. For example, "having a (100) plane preferential orientation" includes not only the case where all the crystals are oriented in the (100) plane, but also the case where more than half of the crystals (in other words, 50% or more, preferably 80% or more) are oriented in the (100) plane.
[0070] Furthermore, the second orientation section 76 only needs to have a lower (100) plane orientation rate than the first orientation section 75, and may of course be oriented in the (100) plane, but may not be oriented in the (100) plane. In this embodiment, the second orientation section 76 has a (111) plane preferential orientation. That is, the piezoelectric layer 70 in the second region S2 has a (111) plane preferential orientation. Furthermore, the second orientation section 76 may have a (110) plane preferential orientation. That is, the piezoelectric layer 70 in the second region S2 may have a (110) plane preferential orientation.
[0071] As described in more detail below, since the piezoelectric layer 70 has the first orientation section 75 and the second orientation section 76, a surface layer section 700 having a different titanium content between the first orientation section 75 and the second orientation section 76 exists near the surface of the piezoelectric layer 70 on the first electrode 60 side. That is, the piezoelectric layer 70 has the surface layer section 700, at least on the first electrode 60 side, having a different titanium content between the first region S1 and the second region S2.
[0072] In this way, the piezoelectric layer 70 has the first orientation section 75 and the second orientation section 76, so that the generation of heat in the piezoelectric layer 70 can be suppressed while suppressing the inhibition of the deformation of the piezoelectric actuator 300. The first orientation section 75, which has a (100) plane preferential orientation, has a relatively large piezoelectric strain when a voltage is applied. On the other hand, for example, the second orientation section 76, which has a (111) plane preferential orientation and has a lower (100) plane orientation rate than the first orientation section 75, has a smaller piezoelectric strain when a voltage is applied to the piezoelectric actuator 300 than the first orientation section 75. Therefore, the piezoelectric layer 70 has the second orientation section 76 in the region outside the pressure chamber 12, so that the generation of heat in the piezoelectric layer 70 can be suppressed while suppressing the inhibition of the deformation of the piezoelectric actuator 300.
[0073] It is preferable that the second orientation section 76 is formed over as wide an area as possible in a non-flexible portion of the active section 310 of the piezoelectric actuator 300, i.e., in a portion extending outside the pressure chamber 12. This makes it possible to more effectively suppress heat generation in the piezoelectric layer 70.
[0074] Also, it is preferable that the end 76b on the -X direction side of the second orientation section 76 is located outside the end 80b on the -X direction side of the second electrode 80. That is, it is preferable that the piezoelectric layer 70 in the second region S2, which has a lower (100) orientation rate than the piezoelectric layer 70 in the first region S1, extends to the outside of the end 80b of the second electrode 80. Furthermore, it is preferable that the end 76b on the -X direction side of the second orientation section 76 is located at a position somewhat away from the end 80b on the -X direction side of the second electrode 80.
[0075] The end 80b of the second electrode 80 defines the boundary between the active section 310 where piezoelectric strain occurs when a voltage is applied and the inactive section 320 where no piezoelectric strain occurs. For this reason, cracks and the like are likely to occur in the piezoelectric layer 70 near the end 80b of the second electrode 80 when a voltage is applied. However, by extending the second orientation section 76 to the outside beyond the end 80b of the second electrode 80, the piezoelectric strain of the active section 310 is also suppressed to be small. Therefore, the occurrence of cracks in the piezoelectric layer 70 near the end 80b of the second electrode 80 can be suppressed.
[0076] 6, the end 76b of the second orientation portion 76 may be located on the +X direction side of the end 80b of the second electrode 80. In such a configuration, the effect of suppressing the occurrence of cracks in the piezoelectric layer 70 near the end 80b of the second electrode 80 may be low, but the effect of suppressing heat generation in the piezoelectric layer 70 can be obtained.
[0077] On the other hand, the position of the end 76a on the +X direction side of the second alignment section 76 is not particularly limited, but is preferably in the vicinity of the end 12b of the pressure chamber 12. Furthermore, as long as the displacement amount of the piezoelectric actuator 300 due to the application of a voltage can be secured, the end 76a on the +X direction side of the second alignment section 76 may be located within the pressure chamber 12 as shown in Fig. 7. By making the range of the second alignment section 76 as wide as possible in this manner, heat generation in the piezoelectric layer 70 can be further suppressed.
[0078] However, it is preferable that the end 76a of the second orientation section 76 on the +X direction side, i.e., the boundary between the first orientation section 75 and the second orientation section 76, is located within the region facing the extension section 93 formed on the second electrode 80. Since the first orientation section 75 and the second orientation section 76 have different magnitudes of piezoelectric strain when a voltage is applied, when a voltage is applied to the piezoelectric actuator 300, cracks are likely to occur in the piezoelectric layer 70 near the end 76a of the second orientation section 76, which is the boundary between the first orientation section 75 and the second orientation section 76. However, if the end 76a of the second orientation section 76 is within the region facing the extension section 93, the extension section 93 restricts the displacement of the piezoelectric actuator 300 near the boundary between the first orientation section 75 and the second orientation section 76, so that the occurrence of cracks in the piezoelectric layer 70 can be suppressed.
[0079] In this embodiment, the portion of the piezoelectric layer 70 on the outer side of the second orientation portion 76, i.e., on the -X direction side, is the first orientation portion 75. However, the orientation of this portion of the piezoelectric layer 70 is not particularly limited. The portion of the piezoelectric layer 70 on the -X direction side of the second orientation portion 76 is an inactive portion 320 where the second electrode 80 is not formed, and therefore does not generate heat when a voltage is applied. Therefore, this portion may of course be the second orientation portion 76, or the (100) plane orientation rate may be different from those of the first orientation portion 75 and the second orientation portion 76.
[0080] Next, a description will be given of an example of a method for manufacturing the ink jet recording head 1 according to this embodiment, in particular, an example of a method for manufacturing the piezoelectric actuator 300. Figures 8 to 19 are cross-sectional views showing the method for manufacturing the ink jet recording head.
[0081] First, as shown in Fig. 8, an elastic film 51 is formed on the surface of a flow path forming substrate wafer 110, which is a silicon wafer. In this embodiment, the elastic film 51 made of silicon dioxide is formed by thermally oxidizing the flow path forming substrate wafer 110. Of course, the material of the elastic film 51 is not limited to silicon dioxide, and may be a silicon nitride film, a polysilicon film, an organic film (polyimide, parylene, etc.), etc. The method of forming the elastic film 51 is not limited to thermal oxidation, and may be a sputtering method, a CVD method, a spin coating method, etc.
[0082] 9, an insulating film 52 made of zirconium oxide is formed on the elastic film 51. The insulating film 52 is not limited to zirconium oxide, and titanium oxide (TiO2), aluminum oxide (Al2O3), hafnium oxide (HfO2), magnesium oxide (MgO), lanthanum aluminate (LaAlO3), etc. may be used. Methods for forming the insulating film 52 include sputtering, CVD, and vapor deposition. In this embodiment, the elastic film 51 and the insulating film 52 form the vibration plate 50, but only one of the elastic film 51 and the insulating film 52 may be provided as the vibration plate 50.
[0083] 10, a first electrode 60 is formed on the entire surface of the insulating film 52. The material of the first electrode 60 is not particularly limited, but when lead zirconate titanate (PZT) is used as the piezoelectric layer 70, it is desirable to use a material that has little change in conductivity due to diffusion of lead oxide. For this reason, platinum, iridium, or the like is preferably used as the material of the first electrode 60. The first electrode 60 can be formed by, for example, a sputtering method or a PVD (physical vapor deposition) method.
[0084] 11, a crystal seed layer 61 made of titanium (Ti) is formed as an orientation control layer on the first electrode 60. The crystal seed layer 61 may be formed in a layered shape or an island shape.
[0085] At this time, the crystal seed layer 61a at a position corresponding to the first orientation section 75 and the crystal seed layer 61b at a position where the second orientation section 76 is to be formed are formed to different thicknesses. That is, the crystal seed layer 61a at a position corresponding to the first orientation section 75 is formed to have a thickness in the range of, for example, about 1 to 200 nm, and preferably to a predetermined thickness in the range of about 5 to 20 nm, so that the first orientation section 75 has a (100) plane preferential orientation, and the crystal seed layer 61b at a position where the second orientation section 76 is to be formed is formed to a thickness different from that of the crystal seed layer 61a.
[0086] In the present embodiment, the second orientation portion 76 having the (111) plane preferential orientation is formed by patterning the crystal seed layer 61 formed on the first electrode 60 by etching or the like, and as shown in FIG. 12, the crystal seed layer 61b at the position where the second orientation portion 76 is formed is removed, or the thickness of the crystal seed layer 61b at the position where the second orientation portion 76 is formed is made thinner than the crystal seed layer 61a at the position where the first orientation portion 75 is formed. Note that in FIG. 12, the positions where the first orientation portion 75 and the second orientation portion 76 are formed are shown by virtual lines. In this embodiment, the crystal seed layer 61b is substantially removed, and the crystal seed layer 61 in other regions including the crystal seed layer 61a is left with a predetermined thickness. The method of etching the crystal seed layer 61 is not particularly limited, and may be, for example, an etching solution or dry etching such as ion milling.
[0087] In the crystal seed layer 61a formed to a predetermined thickness, when the piezoelectric layer 70 is formed in a later step, the preferred orientation direction of the piezoelectric layer 70 can be controlled to (100), and a first orientation portion 75 of the piezoelectric layer 70 suitable for an electromechanical conversion element can be obtained. On the other hand, in the crystal seed layer 61b that is removed or left thin, when the piezoelectric layer 70 is formed in a later step, the piezoelectric layer 70 grows under the influence of the first electrode 60, which is the underlayer. The first electrode 60, which is the underlayer, is made of, for example, platinum or the like and has a (111) plane preferred orientation, so that the second orientation portion 76 has a (111) plane preferred orientation under the influence of the first electrode 60.
[0088] Here, the crystal seed layer 61 functions as a seed that promotes crystallization when the piezoelectric layer 70 crystallizes, and diffuses into the piezoelectric layer 70 after the piezoelectric layer 70 is fired. Therefore, the piezoelectric layer 70 has a surface layer 700 in which the titanium content differs between the first orientation portion 75 and the second orientation portion 76 near the surface on the first electrode 60 side, for example, in a range of about 20 nm to 30 nm. That is, the piezoelectric layer 70 has a surface layer 700 on the first electrode 60 side in which the titanium content differs between the first region S1 and the second region S2 (see FIG. 4).
[0089] Specifically, the titanium content of the surface layer portion 700b formed in the second orientation portion 76 having the (111) plane preferred orientation is lower than the titanium content of the surface layer portion 700a of the first orientation portion 75 having the (100) plane preferred orientation. That is, the titanium content of the surface layer portion 700b in the second region S2 is lower than the titanium content of the surface layer portion 700a in the first region S1.
[0090] That is, the first orientation section 75 has a surface layer portion 700a containing a predetermined amount of titanium as a result of having a (100) plane preferred orientation, and the second orientation section 76 has a surface layer portion 700b having a lower titanium content than the surface layer portion 700a of the first orientation section 75 as a result of having a (111) plane preferred orientation. Note that "low titanium content" is a relative definition, and the surface layer portion 700b of the second orientation section 76 does not necessarily need to contain titanium.
[0091] Incidentally, unlike the present embodiment, when forming the second orientation section 76 having the (110) plane preferential orientation, the thickness of the crystal seed layer 61b at the position corresponding to the second orientation section 76 is made thicker than the thickness of the crystal seed layer 61a at the position corresponding to the first orientation section 75. For example, the crystal seed layer 61 formed on the first electrode 60 is patterned by etching or the like to once remove the crystal seed layer 61a at the position corresponding to the first orientation section 75. Thereafter, the crystal seed layer 61 made of titanium (Ti) is formed again on the first electrode 60 with a predetermined thickness. As a result, the crystal seed layer 61a at the position corresponding to the first orientation section 75 has an appropriate thickness, and the crystal seed layer 61b at the position facing the second orientation section 76 is thicker than the crystal seed layer 61a.
[0092] Even in this case, in the portion of the crystal seed layer 61a provided with a predetermined thickness, when the piezoelectric layer 70 is formed in a later step, the preferred orientation direction of the piezoelectric layer 70 can be controlled to (100), and a first orientation portion 75 of the piezoelectric layer 70 suitable for an electromechanical conversion element can be obtained. On the other hand, in the portion of the crystal seed layer 61b formed thicker than the crystal seed layer 61a, when the piezoelectric layer 70 is formed in a later step, the piezoelectric layer 70 grows freely and the second orientation portion 76 has a (110) plane preferred orientation.
[0093] Also in this case, the piezoelectric layer 70 has a surface portion 700 in which the titanium content differs between the first orientation portion 75 and the second orientation portion 76, near the surface on the first electrode 60 side. The titanium content of the surface portion 700b of the second orientation portion 76, which has a (110) plane preferential orientation, is higher than the titanium content of the surface portion 700a of the first orientation portion 75. That is, the titanium content of the surface portion 700b in the second region S2 is higher than the titanium content of the surface portion 700b in the first region S1.
[0094] In other words, the first orientation portion 75 has a surface portion 700a that contains a predetermined amount of titanium as a result of having a (100) plane preferred orientation, and the second orientation portion 76 has a surface portion 700b that has a higher titanium content than the surface portion 700a of the first orientation portion 75 as a result of having a (110) plane preferred orientation.
[0095] Next, the piezoelectric layer 70 made of lead zirconate titanate (PZT) is formed. In this embodiment, the piezoelectric layer 70 is formed by a so-called sol-gel method, in which a so-called sol in which a metal complex is dissolved and dispersed in a solvent is applied, dried, gelled, and then fired at a high temperature to obtain the piezoelectric layer 70 made of a metal oxide. The method for producing the piezoelectric layer 70 is not limited to the sol-gel method, and may be, for example, a liquid phase film formation method such as an MOD method, or a gas phase film formation method such as a sputtering method, a physical vapor deposition method (PVD method), or a laser ablation method.
[0096] As a specific procedure for forming the piezoelectric layer 70, first, as shown in FIG. 13, a piezoelectric precursor film 73, which is a PZT precursor film, is formed on the first electrode 60 on which the crystal seed layer 61 is formed. That is, a sol (solution) containing a metal complex is applied onto the flow path forming substrate wafer 110 on which the first electrode 60 (crystal seed layer 61) is formed (application step). Next, the piezoelectric precursor film 73 is heated to a predetermined temperature and dried for a certain period of time (drying step). For example, in this embodiment, the piezoelectric precursor film 73 can be dried by holding it at 170 to 180° C. for 8 to 30 minutes.
[0097] Next, the dried piezoelectric precursor film 73 is degreased by heating to a predetermined temperature and holding for a certain period of time (degreasing step). For example, in this embodiment, the piezoelectric precursor film 73 is degreased by heating to a temperature of about 300 to 400°C and holding for about 10 to 30 minutes. Note that degreasing here refers to removing organic components contained in the piezoelectric precursor film 73 as, for example, NO2, CO2, H2O, etc.
[0098] 14, the piezoelectric precursor film 73 is heated to a predetermined temperature and maintained for a certain period of time to be crystallized, forming a piezoelectric film 74 (firing process). In this firing process, the piezoelectric precursor film 73 is preferably heated to 700° C. or higher. In addition, in the firing process, the temperature rise rate is preferably set to 50° C. / sec or higher. This makes it possible to obtain a piezoelectric film 74 with excellent characteristics.
[0099] As a heating device used in such drying, degreasing and baking steps, for example, a hot plate or an RTP (Rapid Thermal Processing) device that heats by irradiating with an infrared lamp can be used.
[0100] 15, at the stage where the first-layer piezoelectric film 74 is formed on the first electrode 60, the first electrode 60 and the first-layer piezoelectric film 74 are simultaneously patterned. Note that the patterning of the first electrode 60 and the first-layer piezoelectric film 74 can be performed by dry etching such as ion milling.
[0101] Here, for example, when the first electrode 60 is patterned and then the first piezoelectric film 74 is formed, the first electrode 60 is patterned by a photo process, ion milling, and ashing, and therefore the surface of the first electrode 60 is altered. If this occurs, even if a piezoelectric film 74 is formed on the altered surface, the crystallinity of the piezoelectric film 74 will not be good, and the second and subsequent piezoelectric films 74 will also grow in crystal form while being influenced by the crystalline state of the first piezoelectric film 74, making it impossible to form a piezoelectric layer 70 with good crystallinity.
[0102] In contrast, if the first piezoelectric film 74 is formed and then patterned simultaneously with the first electrode 60, the first piezoelectric film 74 has stronger properties as a seed for favorable crystal growth of the second and subsequent piezoelectric films 74 than the first electrode 60, etc., and even if an extremely thin altered layer is formed on the surface by patterning, it does not significantly affect the crystal growth of the second and subsequent piezoelectric films 74.
[0103] Next, as shown in FIG. 16, the piezoelectric film formation process, which is comprised of the above-mentioned coating step, drying step, degreasing step and firing step, is repeated a number of times to form a piezoelectric layer 70 comprised of a number of piezoelectric films 74.
[0104] 17, the piezoelectric layer 70 is patterned to correspond to each pressure chamber 12. In this embodiment, a mask (not shown) formed in a predetermined shape is provided on the piezoelectric layer 70, and the piezoelectric layer 70 is etched through this mask, that is, patterning is performed by so-called photolithography. The piezoelectric layer 70 can be patterned by dry etching such as reactive ion etching and ion milling, for example.
[0105] 18, a second electrode 80 made of, for example, iridium (Ir) is formed over the piezoelectric layer 70 and the insulator film 52, and the second electrode 80 is patterned into a predetermined shape. Furthermore, as shown in FIG 19, an individual lead electrode 91 and a common lead electrode 92 are formed on the flow path forming substrate wafer 110. In this way, a piezoelectric actuator 300 is formed.
[0106] Although subsequent steps are not shown in the drawings, a protective substrate wafer, which is a silicon wafer and serves as a plurality of protective substrates 30, is bonded to the piezoelectric actuator 300 side of the flow path forming substrate wafer 110, and then the flow path forming substrate wafer 110 is thinned to a predetermined thickness. In addition, the flow path forming substrate wafer 110 is anisotropically etched (wet etched) using an alkaline solution such as KOH through a mask film patterned into a predetermined shape, thereby forming pressure chambers 12 partitioned by partition walls 11.
[0107] Furthermore, unnecessary portions of the outer periphery of the flow path forming substrate wafer 110 and the protective substrate wafer are removed by, for example, cutting by dicing. Then, the bonded body of the flow path forming substrate wafer 110 and the protective substrate wafer is divided into flow path forming substrates 10 each having a chip size as shown in Fig. 1. Then, the communication plate 15, the nozzle plate 20, the case member 40, the compliance substrate 45, etc. are bonded to the bonded body of the protective substrate 30 and the flow path forming substrate 10, thereby manufacturing the recording head 1 of this embodiment.
[0108] As described above, in the ink jet recording head 1 according to this embodiment, the piezoelectric layer 70 in the first region S1 has a (100) plane preferential orientation, and the (100) plane orientation rate of the piezoelectric layer 70 in the second region S2 is lower than the (100) plane orientation rate of the piezoelectric layer 70 in the first region S1. More specifically, in the recording head 1, the piezoelectric layer 70 has a first orientation portion 75 having a (100) plane preferential orientation in the first region S1, and a second orientation portion 76 having a (111) plane preferential orientation in the second region S2. This makes it possible to suppress heat generation in the piezoelectric layer 70 while suppressing inhibition of deformation of the piezoelectric actuator 300.
[0109] In this embodiment, the process of forming the piezoelectric actuator 300 includes a process of forming the crystal seed layer 61, which is an orientation control layer for controlling the crystal orientation of the piezoelectric layer 70. In the process of forming the crystal seed layer 61, the crystal seed layer 61 is formed to have different thicknesses in the first region S1 and the second region S2. That is, the crystal seed layer 61 is formed to have different thicknesses in the first orientation section 75 and the second orientation section 76. Specifically, as described above, the thickness of the crystal seed layer 61 at the position corresponding to the second orientation section 76 is made thinner than the thickness of the crystal seed layer 61 at the position corresponding to the first orientation section 75. This allows the first orientation section 75 to be preferentially oriented in the (100) plane, and the second orientation section 76 to be preferentially oriented in the (111) plane.
[0110] In this embodiment, when forming the piezoelectric layer 70, the orientation of the piezoelectric layer 70, i.e., the orientation of the first orientation portion 75 and the second orientation portion 76, is controlled by adjusting the thickness of the crystal seed layer 61 serving as an orientation control layer formed on the first electrode 60. However, the orientation of the piezoelectric layer 70 can also be controlled by adjusting the thickness of a so-called intermediate crystal seed layer.
[0111] After the first piezoelectric film 74 and the first electrode 60 are patterned (see FIG. 15), the intermediate crystal seed layer 62 is formed over the insulating film 52, the side surface of the first electrode 60, the side surface of the first piezoelectric film 74, and the piezoelectric film 74, as shown in FIG. 20. This intermediate crystal seed layer 62 is preferably made of titanium, as with the crystal seed layer 61, and is formed in a layer or island shape. Thereafter, the second and subsequent piezoelectric films 74 are formed as in the above-described embodiment (see FIGS. 16 to 19).
[0112] The orientation of the second and subsequent piezoelectric films 74 can also be controlled by the intermediate crystal seed layer 62. As in the case of the above-mentioned crystal seed layer 61, the thickness of the intermediate crystal seed layer 62b at the position corresponding to the second orientation portion 76 is made thinner than the thickness of the intermediate crystal seed layer 62a at the position corresponding to the first orientation portion 75 (see FIG. 20). This allows the first orientation portion 75 to be preferentially oriented in the (100) plane, and the second orientation portion 76 to be preferentially oriented in the (111) plane. When the intermediate crystal seed layer 62 is formed, a surface layer portion 700 in which the titanium content is different between the first orientation portion 75 and the second orientation portion 76 is present near the surface of the piezoelectric layer 70 on the first electrode 60 side.
[0113] When the intermediate crystal seed layer 62 is formed, the crystal seed layer 61 may not be formed, or the crystal seed layer 61 may be formed together with the intermediate crystal seed layer 62. When the crystal seed layer 61 is formed together with the intermediate crystal seed layer 62, the thickness of the crystal seed layer 61 may be approximately uniform throughout.
[0114] (Embodiment 2) 21 is a cross-sectional view of the ink jet recording head according to this embodiment. Note that the same members are given the same reference numerals and overlapping explanations will be omitted.
[0115] In the above-described first embodiment, the crystal seed layer 61 made of titanium is formed as an orientation control layer during the manufacture of the piezoelectric actuator 300, and as a result, the piezoelectric layer has a titanium-containing surface layer portion 700. In the present embodiment, the crystal seed layer 61 is not formed during the manufacture of the piezoelectric actuator 300, and therefore the titanium-containing surface layer portion 700 does not exist.
[0116] In the ink jet recording head 1 according to this embodiment, as shown in Fig. 21, an orientation layer 150 is provided as an orientation control layer between the first electrode 60 and the piezoelectric layer 70. The orientation layer 150 is made of LaNi y O x , SrRu y O x , (Ba,Sr)Ti y O x , (Bi,Fe)Ti y Ox At least one selected from the group consisting of LaNi y O x It consists of:
[0117] Furthermore, the length in the Z-axis direction of the alignment layer 150 in the second region S2 is shorter than the length in the Z-axis direction of the alignment layer 150 in the first region S1. That is, the alignment layer 150 corresponding to the first alignment portion 75 of the piezoelectric layer 70 is formed to a predetermined thickness, and the thickness of the alignment layer 150b at a position corresponding to the second alignment portion 76 is thinner than the thickness of the alignment layer 150a at a position corresponding to the first alignment portion 75.
[0118] By forming the piezoelectric layer 70 on the orientation layer 150 of a predetermined thickness, the preferred orientation direction of the piezoelectric layer 70 can be controlled to (100), and the piezoelectric layer 70 suitable as an electromechanical transducer can be obtained. Therefore, a first orientation section 75 having a (100) plane preferred orientation is formed on the orientation layer 150 of a predetermined thickness. On the other hand, when the piezoelectric layer 70 is formed on the orientation layer 150 formed thinner than the portion corresponding to the first orientation section 75, it grows under the influence of the first electrode 60, which is the underlayer. The first electrode 60, which is the underlayer, is made of, for example, platinum or the like and has a (111) plane preferred orientation. Therefore, a second orientation section 76 having a (111) plane preferred orientation is formed on the orientation layer 150 formed thinner than the portion corresponding to the first orientation section 75.
[0119] The alignment layer 150 may be formed in the same manner as the crystal seed layer 61. Specifically, after the alignment layer 150 is formed on the entire surface of the first electrode 60, the alignment layer 150 may be patterned by etching or the like to remove the alignment layer 150b at the position corresponding to the second alignment section 76, or to make the thickness of the alignment layer 150b thinner than the thickness of the alignment layer 150 at the position corresponding to the first alignment section 75. The method of etching the alignment layer 150 is not particularly limited, and may be, for example, an etching solution or dry etching such as ion milling.
[0120] Furthermore, the alignment layer 150 according to this embodiment remains as a layer without being diffused into the piezoelectric layer 70. The thickness of the alignment layer 150 is not particularly limited, but is preferably about 5 nm to 20 nm, which allows the first alignment portion 75 to be favorably oriented in the (100) plane.
[0121] (Embodiment 3) 22 is a cross-sectional view of an ink jet recording head, which is an example of a liquid jet head according to a third embodiment of the present invention, and is an enlarged view showing the configuration of a piezoelectric actuator 300. Note that the same members as those in the first embodiment are given the same reference numerals, and duplicated explanations will be omitted.
[0122] 22, the piezoelectric actuator 300 according to this embodiment includes a protective film 200 provided on the -Z direction side of the second electrode 80, i.e., on the second electrode 80. The protective film 200 covers the end 80b of the second electrode 80 close to the second region S2. In other words, the protective film 200 is provided so as to cover the boundary between the active section 310 and the inactive section 320 of the piezoelectric actuator 300. The configuration other than the protective film 200 is the same as that of the first embodiment.
[0123] In the piezoelectric layer 70 near the boundary between the active section 310 and the inactive section 320, for example, stress concentration may occur due to uneven generation of piezoelectric strain, and as a result, cracks and burn damage caused by these cracks may become noticeable. However, in this embodiment, the protective film 200 is provided so as to cover the boundary between the active section 310 and the inactive section 320, so that the occurrence of cracks and burn damage in this region can be more reliably reduced.
[0124] 22, the protective film 200 is provided only near the end 80b of the second electrode 80, but the area where the protective film 200 is formed is not particularly limited. For example, the protective film 200 may be provided so as to cover the exposed portion of the surface of the piezoelectric layer 70 in the inactive portion 320.
[0125] The material of the protective film 200 is not particularly limited, and may be, for example, an organic material such as polyimide (aromatic polyimide). The protective film 200 may be formed of an epoxy-based adhesive or a silicon-based adhesive. When the protective film 200 is formed of an adhesive, the adhesive for bonding the protective substrate 30 to the flow path forming substrate 10 may function as the protective film 200. That is, the protective substrate 30 may be bonded to the flow path forming substrate 10 at a portion corresponding to the end 80b of the second electrode 80 by an adhesive, and the end 80b of the second electrode 80 may be covered by the adhesive.
[0126] Moreover, the Young's modulus of the protective film 200 is preferably lower than that of the second electrode 80 in the second region S2. In this embodiment, the protective film 200 is formed of an organic material such as polyimide, and therefore the Young's modulus of the protective film 200 is lower than that of the second electrode 80, which is formed of a metal such as iridium. This makes it more difficult for piezoelectric distortion to occur in the piezoelectric layer 70 at the boundary between the active section 310 and the inactive section 320, and also makes it easier to absorb vibrations, so that the occurrence of cracks and burnout in this region can be more reliably reduced.
[0127] (Other embodiments) Although each embodiment of the present invention has been described above, the basic configuration of the present invention is not limited to the above.
[0128] For example, in the above embodiment, the thickness of the crystal seed layer 61, the intermediate crystal seed layer 62, or the orientation layer 150 as the orientation control layer is adjusted to make the (100) orientation rate of the second orientation section 76 lower than that of the first orientation section 75, but the method of adjusting the (100) orientation rate of the first orientation section 75 and the second orientation section 76, i.e., the method of adjusting the (100) orientation rate of the piezoelectric layer 70, is not particularly limited. For example, when forming the piezoelectric layer 70, the (100) orientation rate of the piezoelectric layer 70 can be changed by adjusting the amount of impurities attached to the first electrode 60 or the first piezoelectric film 74. More specifically, when patterning the first electrode 60 or the first piezoelectric film 74 using a mask made of an organic material, a small part of the mask is left in the portion where the second orientation section 76 is to be formed, and the remaining piezoelectric layer 70 is formed in this state. This makes it possible to make the (100) orientation rate of the second orientation section 76 lower than that of the first orientation section 75.
[0129] In the above embodiment, the present invention has been described using as an example the configuration in the vicinity of the end 80b in the -Y direction of the second electrode 80, but the present invention can of course also be applied to the vicinity of the end 80b in the +Y direction of the second electrode 80. When a boundary between the active portion 310 and the inactive portion 320 of the piezoelectric actuator 300 defined by the end 80a of the second electrode 80 exists on the outside of the pressure chamber 12 in the +Y direction, the above-mentioned configuration of the present invention can also be applied to the end 80a side in the +Y direction of the second electrode 80.
[0130] In addition, in each of the above-described embodiments, the first electrode 60 constitutes an individual electrode for each active portion 310, and the second electrode 80 constitutes a common electrode for the plurality of active portions 310, but the first electrode 60 may constitute a common electrode for the plurality of active portions 310, and the second electrode 80 may constitute an individual electrode for each active portion 310. Even in this case, the same effects as those of the above-described embodiments can be obtained.
[0131] The recording head 1 of each of these embodiments is mounted on an ink jet recording apparatus, which is an example of a liquid ejecting apparatus. Fig. 23 is a schematic diagram showing an example of an ink jet recording apparatus, which is an example of a liquid ejecting apparatus according to an embodiment.
[0132] 23, a recording head 1 is provided with a detachable cartridge 2 constituting an ink supply means, and is mounted on a carriage 3. The carriage 3 carrying the recording head 1 is provided so as to be freely movable in the axial direction of a carriage shaft 5 attached to a device main body 4.
[0133] The driving force of the drive motor 6 is transmitted to the carriage 3 via multiple gears and a timing belt 7 (not shown), causing the carriage 3 carrying the recording head 1 to move along a carriage shaft 5. Meanwhile, the device body 4 is provided with transport rollers 8 as a transport means, and a recording sheet S, which is a recording medium such as paper, is transported by the transport rollers 8. Note that the transport means for transporting the recording sheet S is not limited to transport rollers, and may be a belt, a drum, or the like.
[0134] In such an inkjet recording device I, the recording sheet S is transported in the +X direction relative to the recording head 1, and the carriage 3 is moved back and forth in the Y direction relative to the recording sheet S, while ink droplets are ejected from the recording head 1, causing the ink droplets to land over almost the entire surface of the recording sheet S, thereby performing so-called printing.
[0135] In addition, in the above-mentioned ink jet recording device I, an example has been given of the recording head 1 mounted on a carriage 3 and moving back and forth in the Y direction, which is the main scanning direction, but the present invention is not limited to this. For example, the present invention can also be applied to a so-called line type recording device in which the recording head 1 is fixed and printing is performed simply by moving a recording sheet S, such as paper, in the X direction, which is the sub-scanning direction.
[0136] In the above embodiment, an ink jet recording head is used as an example of a liquid jet head, and an ink jet recording device is used as an example of a liquid jet device, but the present invention is intended for a wide range of liquid jet heads and liquid jet devices in general, and can of course be applied to liquid jet heads and liquid jet devices that jet liquids other than ink. Other liquid jet heads include, for example, various recording heads used in image recording devices such as printers, color material jet heads used in manufacturing color filters for liquid crystal displays, electrode material jet heads used in forming electrodes for organic EL displays, FEDs (field emission displays), and bioorganic material jet heads used in biochip manufacturing, and can also be applied to liquid jet devices equipped with such liquid jet heads.
[0137] Furthermore, the present invention can be applied not only to liquid ejecting heads such as ink jet recording heads, but also to ultrasonic devices such as ultrasonic transmitters, ultrasonic motors, pressure sensors, pyroelectric sensors and other piezoelectric devices. [Explanation of symbols]
[0138] S1...first region, S2...second region, I...ink-jet recording device (recording device), 1...ink-jet recording head (recording head), 2...cartridge, 3...carriage, 4...device body, 5...carriage shaft, 6...drive motor, 7...timing belt, 8...transport roller, 10...flow path forming substrate (substrate), 11...partition wall, 12...pressure chamber (recess), 15...communication plate, 16...nozzle communication passage, 17...first manifold portion, 18...second manifold portion, 19...supply communication passage, 20...nozzle plate, 21...nozzle, 30...protective substrate, 31...holding portion, 32...through hole, 40...case member, 41...accommodation portion, 42...third manifold portion, 43...connection port, 44...inlet port, 45...convex portion a piezoelectric layer having a first electrode, a second electrode, a common lead electrode, a first layer, a second electrode, a third layer, a wiring portion, a first lead electrode, a first electrode, a first layer, a second electrode, a third layer, a wiring portion, a first electrode, a first layer, a second electrode, a first layer, a first layer, a second layer, a third layer, a second layer, a third layer, a third layer, a third layer, a fourth layer, a fourth layer, a fourth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a fifth layer, a sixth layer, a sixth layer, a sixth layer, a sixth layer, a fifth layer, a sixth layer, a sixth layer, a sixth layer, a sixth layer, a sixth layer, a sixth layer, a seventh ...
Claims
1. A substrate having a plurality of recesses formed therein; A diaphragm provided on one surface side of the substrate; a first electrode and a piezoelectric layer laminated in a first direction on a surface of the vibration plate opposite to the substrate; a piezoelectric actuator having a second electrode, When one of two regions of the second electrode in a second direction intersecting with the first direction is defined as a first region, and the other region closer to the end of the second electrode is defined as a second region, the piezoelectric layer in the first region has a (100) plane preferential orientation, and the (100) plane orientation rate of the piezoelectric layer in the second region is lower than the (100) plane orientation rate of the piezoelectric layer in the first region; the first region is in a driving region where the diaphragm contacts the recess and in a non-driving region where the diaphragm does not contact the recess, the second region is in the non-driven region, a boundary between the first region and the second region in the second direction is located in the non-driven region. A piezoelectric device characterized by:
2. The piezoelectric actuator has a third electrode laminated on the second electrode so as to cover a portion of the second electrode in the first direction and extending in a third direction intersecting the first direction and the second direction; a boundary between the first region and the second region in the second direction is located in a region in which the third electrode is provided, 2. The piezoelectric device according to claim 1 .
3. Between the first electrode and the piezoelectric layer, y O x , SrRuyO x , (Ba,Sr)Ti y O x , (Bi,Fe)Ti y O x An alignment layer including at least one selected from the group consisting of The length of the alignment layer in the second region in the first direction is shorter than the length of the alignment layer in the first region in the first direction.
3. The piezoelectric device according to claim 1, wherein the piezoelectric element is a piezoelectric material.
4. The orientation layer is LaNi y O x Consists of:
4. The piezoelectric device according to claim 3.
5. the piezoelectric layer has a surface layer portion on the first electrode side, the surface layer portion having a different titanium content between the first region and the second region; 3. The piezoelectric device according to claim 1, wherein the piezoelectric element is a piezoelectric material.
6. a titanium content of the surface layer portion in the second region is higher than a titanium content of the surface layer portion in the first region; 6. The piezoelectric device according to claim 5.
7. The piezoelectric layer in the second region has a (110) plane preferential orientation.
7. The piezoelectric device according to claim 6.
8. a titanium content of the surface layer portion in the second region is lower than a titanium content of the surface layer portion in the first region; 6. The piezoelectric device according to claim 5.
9. The piezoelectric layer in the second region has a (111) plane preferential orientation.
9. The piezoelectric device according to claim 8.
10. The piezoelectric layer in the second region extends to an outside of an end of the second electrode.
10. The piezoelectric device according to claim 1, wherein the piezoelectric element is a piezoelectric material.
11. a protective film covering an end of the second electrode close to the second region; 11. The piezoelectric device according to claim 1, wherein the piezoelectric element is a piezoelectric material.
12. A substrate having a plurality of recesses formed therein; A diaphragm provided on one surface side of the substrate; a first electrode and a piezoelectric layer laminated in a first direction on a surface of the vibration plate opposite to the substrate; a piezoelectric actuator having a second electrode, When one of two regions of the second electrode in a second direction intersecting with the first direction is defined as a first region, and the other region closer to the end of the second electrode is defined as a second region, the piezoelectric layer in the first region has a (100) plane preferential orientation, and the (100) plane orientation rate of the piezoelectric layer in the second region is lower than the (100) plane orientation rate of the piezoelectric layer in the first region; the first region is in a driving region where the diaphragm contacts the recess and in a non-driving region where the diaphragm does not contact the recess, the second region is in the non-driven region, a boundary between the first region and the second region in the second direction is located in the non-driven region. A liquid jet head comprising:
13. The piezoelectric actuator has a third electrode laminated on the second electrode so as to cover a portion of the second electrode in the first direction and extending in a third direction intersecting the first direction and the second direction; a boundary between the first region and the second region in the second direction is located in a region in which the third electrode is provided, The liquid jet head according to claim 12 .
14. The liquid jet head according to claim 12 or 13, A liquid ejection apparatus comprising:
15. A substrate having a plurality of recesses formed therein; A diaphragm provided on one surface side of the substrate; a first electrode and a piezoelectric layer laminated in a first direction on a surface of the vibration plate opposite to the substrate; a piezoelectric actuator having a second electrode; When one of two regions of the second electrode in a second direction intersecting with the first direction is defined as a first region, and the other region closer to the end of the second electrode is defined as a second region, a piezoelectric layer in the first region has a (100) plane preferential orientation, a (100) plane orientation rate of the piezoelectric layer in the second region is lower than a (100) plane orientation rate of the piezoelectric layer in the first region, the first region is located in a driving region where the vibration plate contacts a recess and a non-driving region where the vibration plate does not contact the recess, the second region is located in the non-driving region, and a boundary between the first region and the second region in the second direction is located in the non-driving region, forming the piezoelectric actuator by laminating the first electrode, the piezoelectric layer, and the second electrode on a surface of the vibration plate provided on the substrate, the method includes forming an orientation control layer for controlling a crystal orientation of the piezoelectric layer; In the step of forming the orientation control layer, The orientation control layer is formed to have different thicknesses in the first region and the second region. A method for manufacturing a piezoelectric device comprising the steps of:
16. In the step of forming the orientation control layer, After forming the alignment control layer in a region including the first region and the second region on the surface of the first electrode, at least a portion of the alignment control layer in the second region is removed to make the thickness of the alignment control layer in the second region thinner than the thickness of the alignment control layer in the first region. The method for manufacturing a piezoelectric device according to claim 15 .
17. In the step of forming the orientation control layer, forming the alignment control layer in a region including the first region and the second region on the surface of the first electrode, removing at least a portion of the alignment control layer in the first region to make the thickness of the alignment control layer thinner than that of the second region, and then forming the alignment control layer again in the region including the first region and the second region on the surface of the first electrode to make the thickness of the alignment control layer in the second region thicker than that of the alignment control layer in the first region. The method for manufacturing a piezoelectric device according to claim 15 .
Citation Information
Patent Citations
Liquid injection head, liquid injection device and piezoelectric element
JP2013118232A
Liquid ejecting head, liquid ejecting apparatus, and actuator
JP2014058169A
Liquid ejection head, manufacturing method of the same, liquid ejection device and actuator device
JP2015147331A
Liquid injection head and liquid injection device
JP2015171809A
Piezoelectric film, piezoelectric device, and method for producing piezoelectric film
JP2017063138A