Radiation imaging panel, radiation imaging device, radiation imaging system, and scintillator plate
The radiation imaging panel enhances MTF and DQE by using a resin layer with specific thickness and particle concentration of metal oxide particles, addressing light reflection and moisture-proofing issues.
Patent Information
- Application Number
- JP2020120869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-14
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-07-14
AI Technical Summary
Existing radiation imaging panels face challenges in improving Modulation Transfer Function (MTF) due to inadequate dispersion concentration and thickness of light-reflecting fine particles in the protective layer, leading to insufficient light reflection and moisture-proofing issues.
A radiation imaging panel with a protective layer comprising a resin doped with metal oxide particles, where the resin layer thickness is 10 μm or more and less than 30 μm, and the particle concentration is 0.15 vol% or more and less than 7.5 vol%, enhancing light reflection and moisture-proofing.
The solution improves MTF characteristics while maintaining Detective Quantum Efficiency (DQE) by optimizing the resin layer thickness and particle concentration, resulting in efficient light utilization and protection against moisture.
Smart Images

Figure 0007564655000001 
Figure 0007564655000002 
Figure 0007564655000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a radiation imaging panel, a radiation imaging device, a radiation imaging system, and a scintillator plate. [Background technology]
[0002] As a flat panel detector (FPD) used for radiography in medical image diagnosis and non-destructive testing, there is an indirect conversion type FPD in which radiation passing through a subject is converted into light by a scintillator, and the light emitted by the scintillator is detected by a photoelectric conversion element. For the scintillator that converts radiation into light, columnar crystals of alkali metal halide compounds such as cesium iodide are widely used in order to efficiently transmit the light converted from radiation to the photoelectric conversion element. Since the alkali metal halide compounds deteriorate due to moisture absorption, a protective layer having a moisture-proof function may be arranged on the scintillator. In addition, a reflective layer having a light-reflecting function may be arranged on the side of the scintillator opposite the photoelectric conversion element so that the light converted from radiation by the scintillator is efficiently detected by the photoelectric conversion element. Patent Document 1 shows a radiation detection device having a phosphor protective layer made of a resin containing light-reflective fine particles having a moisture-proof function and a light-reflecting function for the phosphor layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-052980 A Summary of the Invention [Problem to be solved by the invention]
[0004] The dispersion concentration of the light-reflective fine particles shown in Patent Document 1 needs to be considered. Specifically, if the concentration of the light-reflective fine particles is too low, the effect of reflecting light becomes insufficient, and the effect of improving the MTF (Modulation Transfer Function) may be insufficient. On the other hand, Patent Document 1 shows that a metal oxide such as TiO2 that transmits light incident at a critical angle or less is used as the light-reflective fine particles, but if the concentration of the light-reflective fine particles is too high, the probability that light will be incident on the light-reflective fine particles at a narrow angle less than the critical angle increases. Furthermore, if the concentration of the light-reflective fine particles is high and the light-reflective fine particles are in contact with each other, the light that has passed through one light-reflective fine particle may enter the other light-reflective fine particle and the light may be diffused. As a result, the effect of reflecting light becomes insufficient, and the effect of improving the MTF may be insufficient.
[0005] There is also room for consideration regarding the thickness of the phosphor protective layer in which the light-reflective particles are dispersed. If the phosphor protective layer is too thick, the light will be diffused within the phosphor protective layer, and the MTF improvement effect may be insufficient. Also, if the protective layer is too thin, the moisture-proof function may be insufficient.
[0006] An object of the present invention is to provide a technique that is advantageous for improving the MTF in a radiation imaging panel. [Means for solving the problem]
[0007] In view of the above problems, a radiation imaging panel according to an embodiment of the present invention is a radiation imaging panel including a substrate on which a plurality of pixels, each of which includes a photoelectric conversion element, is arranged, a scintillator arranged on the substrate, and a protective layer arranged to cover the scintillator, wherein the scintillator includes a plurality of columnar crystals including an alkali metal halide compound, and the protective layer is a resin layer including a resin to which metal oxide particles are added. a base disposed on a side of the resin layer opposite to the scintillator; and a metal layer disposed between the resin layer and the base. Equipped with The resin includes a hot melt resin,The resin layer is characterized in that the thickness from the top of each of the plurality of columnar crystals to the upper surface of the resin layer is 10 μm or more and less than 30 μm, and the concentration of the particles in the resin layer is 0.15 vol% or more and less than 7.5 vol%. Effect of the Invention
[0008] The above-mentioned means provides a technique that is advantageous for improving the MTF in a radiation imaging panel. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view showing an example of the configuration of a radiation imaging panel according to the present embodiment. [Diagram 2] 2 is a cross-sectional view showing an example of the configuration of a protective layer of the radiation imaging panel shown in FIG. 1. [Diagram 3] 2 is a graph showing characteristics of the radiation imaging panel of FIG. 1; [Figure 4] 2 is a graph showing characteristics of the radiation imaging panel of FIG. 1; [Diagram 5] FIG. 2 is a SEM image of a cross section of the radiation imaging panel of FIG. 1. [Figure 6] 2 is a graph showing characteristics of the radiation imaging panel of FIG. 1; [Figure 7] 2 is a graph showing characteristics of the radiation imaging panel of FIG. 1; [Figure 8] 2 is a diagram showing an example of the configuration of a radiation imaging apparatus and a radiation imaging system using the radiation imaging panel of FIG. 1; [Figure 9] 2A to 2C are diagrams for explaining a problem with the resin layer of the radiation imaging panel of FIG. 1; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments will be described in detail with reference to the attached drawings. Note that the following embodiments do not limit the invention according to the claims. Although the embodiments describe a number of features, not all of these features are essential to the invention, and the features may be combined in any manner. Furthermore, in the attached drawings, the same reference numbers are used for the same or similar configurations, and duplicated descriptions are omitted.
[0011] Furthermore, radiation in the present invention may include α-rays, β-rays, γ-rays, and other beams produced by particles (including photons) emitted by radioactive decay, as well as beams having the same or greater energy, such as X-rays, particle beams, and cosmic rays.
[0012] The configuration of a radiation imaging panel according to this embodiment will be described with reference to Figures 1(a) to 9(b). Figure 1(a) is a diagram showing a cross-sectional structure of a radiation imaging panel 100 according to this embodiment. Figure 1(b) is an enlarged view of a portion 111 in Figure 1(a).
[0013] The radiation imaging panel 100 includes a substrate 101 having a pixel region 105 in which a plurality of pixels each including a photoelectric conversion element are arranged, a scintillator 108 arranged on the substrate 101, and a protective layer 110 arranged so as to cover the scintillator 108. The scintillator 108 includes a plurality of columnar crystals 102 including an alkali metal halide compound. The protective layer 110 includes a resin layer 104 including a resin 103 to which metal oxide particles 106 have been added. A pixel protective layer 107 for protecting the pixels arranged in the pixel region 105 may be arranged between the substrate 101 and the scintillator 108.
[0014] In the pixel region 105, a plurality of pixels may be arranged in a two-dimensional array. For example, 3300×2800 pixels may be arranged on the substrate 101 of 550 mm×445 mm. Ten pixels arranged on the outer periphery of the 3300×2800 pixels may be a dummy pixel region, and the effective pixel region of the pixel region 105 may be composed of 3280×2780 pixels arranged inside the dummy pixels. The number of pixels arranged in the pixel region 105 and the number of pixels arranged in the effective pixel region of the pixel region 105 may be appropriately set according to the size of the substrate 101, the subject to be imaged, and the like.
[0015] In the pixel region 105, column signal lines for extracting signals generated in each pixel and row signal lines for driving each element including the pixels arranged in the pixel region 105 may be arranged. The column signal lines and row signal lines may be electrically connected to a readout circuit board and a drive circuit board via a flexible wiring board or the like. In order to connect the column signal lines and row signal lines to the readout circuit board and the drive circuit board, the substrate 101 may be provided with a connection terminal portion (not shown). A signal generated in each pixel in the pixel region 105 may be output from the radiation imaging panel 100 via the connection terminal portion.
[0016] Here, an example is shown in which the readout circuit and the drive circuit are disposed outside the radiation imaging panel 100, but the readout circuit and the drive circuit may be disposed in the radiation imaging panel 100. Even in this case, a connection terminal portion (not shown) is disposed on the substrate 101, and a signal generated in each pixel of the pixel region 105 can be output from the radiation imaging panel 100 via the connection terminal portion (not shown).
[0017] 1(a), the resin layer 104 having metal oxide particles 106 dispersed in the resin 103 is disposed on the opposite side of the scintillator 108 to the pixel region 105. This makes it possible to efficiently utilize the light generated by the scintillator 108, and the sensitivity of the radiation imaging panel 100 can be improved.
[0018] Furthermore, the scintillator 108 composed of a plurality of columnar crystals 102 containing an alkali metal halide compound deteriorates due to moisture absorption. Therefore, the resin layer 104 in which metal oxide particles 106 are dispersed in the resin 103 may also function as a moisture-proof layer for the scintillator 108. By providing the resin layer 104 covering the scintillator 108 with the function of a moisture-proof layer, it becomes possible to prevent the scintillator 108 from deteriorating due to moisture absorption.
[0019] FIG. 1(b) is a diagram for explaining the function of the resin layer 104 in which metal oxide particles 106 are dispersed in the resin 103. As shown in FIG. 1(b), the light emitted from the columnar crystals of the scintillator 108 toward the resin 103 is specularly reflected or diffusely reflected by the particles 106 present in a dispersed state. A part of the light reflected by the particles 106 returns to the columnar crystals 102 from which it was emitted. Another part of the light reflected by the particles 106 is attenuated by being repeatedly reflected by other particles. In other words, the light is diffused in the resin layer 104, and the light can be prevented from spreading. This shows that a high MTF (Modulation Transfer Function) can be obtained by the resin layer 104 in which the metal oxide particles 106 are dispersed in the resin 103.
[0020] However, as shown in FIG. 9(a), when the number of metal oxide particles 106 is small, the effect of reflection by the particles 106 may not be obtained. On the other hand, as shown in FIG. 9(b), when the concentration of metal oxide particles 106 such as TiO2 that transmit light incident at a critical angle or less is too high, the probability that light will be incident on the particles 106 at a narrow angle less than the critical angle increases. Furthermore, when the concentration of light-reflecting fine particles is high and the light-reflecting fine particles are in contact with each other, the light that has passed through one light-reflecting fine particle will be incident on the other light-reflecting fine particle and the light will be diffused. As a result, the effect of reflecting light may be insufficient, and the effect of improving MTF may be insufficient. The appropriate concentration of metal oxide particles 106 and the thickness of the resin layer 104 will be described later.
[0021] Next, a method for manufacturing the radiation imaging panel 100 will be described. For example, non-alkali glass having a size of 550 mm×445 mm and a thickness of 500 μm may be used as the substrate 101. A pixel region 105 is formed by repeatedly performing a film forming process, a photolithography process, an etching process, and the like on the glass substrate 101. In the pixel region 105, a plurality of pixels each including a photoconversion element that generates a charge according to the light emitted by the scintillator 108 and a switching element that outputs a signal according to the generated charge are arranged. In addition, in the pixel region 105, a connection terminal portion (not shown) for driving the pixel and sending the obtained signal to an external circuit and the like are formed.
[0022] After the pixel region 105 is formed, an array test may be performed to check the operation of the pixels formed in the pixel region 105. After it is confirmed in the array test that the operation is good and there are no or only a few missing pixels, the peripheral portion of the substrate 101 may be masked with a masking film in order to protect a connection terminal portion (not shown), and the pixel protection layer 107 may be formed. The pixel protection layer 107 may be formed, for example, by placing the substrate 101 in a spray spin coater, spinning at a rotation speed of about 100 rpm while spraying a polyimide solution, and then drying and dry annealing at a temperature of 220°C. For example, the pixel protection layer 107 may have a thickness of about 2 μm.
[0023] Next, the scintillator 108 is formed. First, a deposition mask is set on the region of the substrate 101 on which the pixel protection layer 107 is formed, on which the scintillator 108 is not to be formed, and then the substrate 101 is placed on a deposition device so that the pixel protection layer 107 becomes the deposition surface. Then, cesium iodide (CsI) and thallium iodide (TlI) are filled in cell containers so that the Tl concentration is 1 mol % relative to CsI, and co-deposition is performed by heating. The scintillator 108 may have a thickness of, for example, 380 μm and a film filling rate of 75%. At this time, the outer edge of the scintillator 108 may be disposed outside the outer edge of the pixel region 105. In addition, when depositing the scintillator 108, the deposition device is set to 100° C. -3After evacuating the chamber to 100 Pa, the substrate surface may be heated to 175° C. using a lamp heater.
[0024] The protective layer 110 may be fabricated as follows. FIG. 2 is a diagram showing a configuration example of the protective layer 110. In this embodiment, the protective layer 110 is formed by forming an aluminum metal layer 202 on a base 201, and forming a resin layer 104 containing a resin 103 to which metal oxide particles 106 are added on the metal layer 202. The resin layer 104 of the protective layer 110 may be in contact with the scintillator 108. The protective layer 110 is not limited to the three-layer structure shown in FIG. 2. For example, other layers may be laminated on the protective layer 110, such as a resin layer to which metal oxide particles are not added. Also, for example, the protective layer 110 may be only the resin layer 104, or may be a two-layer structure of the resin layer 104 and the metal layer 202.
[0025] In this embodiment, the resin 103 constituting the resin layer 104 is a hot melt resin mainly composed of polyolefin resin. The hot melt resin is defined as an adhesive resin that does not contain water or solvent, is solid at room temperature, and is made of 100% non-volatile thermoplastic material (Thomas P. Flanagan, Adhesives Age, vol. 9, No. 3, pp. 28 (1966)). The hot melt resin has the property of melting when the resin temperature rises and solidifying when the resin temperature drops, and is adhesive to other organic materials and inorganic materials in a heated and molten state, but is in a solid state at room temperature and does not have adhesive properties. In addition, since the hot melt resin does not contain polar solvents, solvents, or water, it does not dissolve the scintillator 108 even when it comes into contact with the scintillator 108 having the columnar crystals 102 of an alkali halide, and therefore can also function as a protective layer.
[0026] Hot melt resins are classified according to the type of base polymer (base material) that is the main component, and polyolefin-based, polyester-based, polyamide-based, etc. can be used. When using a hot melt resin for protective layer 110 of scintillator 108, it is important that the resin has high moisture resistance and high optical transparency for transmitting visible light generated from scintillator 108.
[0027] For example, the resin layer 104 is prepared by dissolving a polyolefin resin as the resin 103 in a mixed solvent of toluene and xylene, and adjusting the viscosity to about 10 cps. Metal oxide particles 106 are also dispersed in advance in a mixed solution of butanol and propanol together with a dispersant. The material in which the polyolefin resin is dissolved in the mixed solution of toluene and xylene is sufficiently crushed by a ball mill to obtain a dispersion liquid, which is then added so that the particles 106 are 0-32 vol% in the resin layer 104, and then mixed. After sufficiently stirring this dispersion liquid, the solvent is volatilized while being careful not to foam, to obtain the resin layer 104.
[0028] The metal oxide particles 106 may be made of a material having a higher refractive index than the scintillator 108. For example, when the above-mentioned CsI (refractive index (n): 1.78 to 1.84 (depending on the type of activator, etc.)) is used as the scintillator 108 of the alkali metal halide compound, a material having a higher refractive index than CsI may be used. For example, the metal oxide particles 106 may contain at least one of white lead (2PbCo3·Pb(OH)2) (n: 1.94 to 2.09), zinc oxide (n: 2.0), yttrium oxide (n: 1.91), zirconium oxide (n: 2.20), and titanium oxide (n: 2.50 to 2.72). For example, the refractive index of the metal oxide particles 106 may be 1.94 or more and 2.72 or less. In this embodiment, the metal oxide will be described as being made of rutile titanium dioxide particles, which have a high refractive index among titanium oxides.
[0029] The average particle size of the metal oxide particles 106 may be 200 nm or more and 500 nm or less. Generally, the sensitivity characteristic of a photoelectric conversion element is 500 nm to 800 nm, but if the particles are 1 / 2 the wavelength of light or less, the effect of Rayleigh scattering appears, and the probability of reflection in the direction of the light incidence increases. In this embodiment, the average particle size is 250 nm, the particle size distribution is 10% diameter D 10 = 195 μm, 50% diameter (median diameter) D 50 =245μm, 90% diameter D 90 Rutile titanium dioxide particles having a diameter of 275 μm are used as the metal oxide particles 106 .
[0030] A PET substrate or the like can be used for the base 201. The protective layer 110 of this embodiment can be obtained by forming a resin layer 104 to which metal oxide particles 106 are added on a film in which an aluminum metal layer 202 having a thickness of 12 μm is formed on a PET base 201 having a thickness of 30 μm. The protective layer 110 can be formed, for example, by setting the base 201 on which the metal layer 202 is formed in a roll coater device, and applying the resin 103 to which the particles 106 prepared as described above are added on the side of the metal layer 202. As a result, the protective layer 110 includes the base 201 arranged on the side opposite the scintillator 108 of the resin layer 104, and further includes the metal layer 202 arranged between the resin layer 104 and the base 201.
[0031] When the inventors actually produced protective layer 110, it was difficult to obtain uniformity in the thickness of resin layer 104 when the thickness of resin layer 104 was less than 10 μm. In other words, resin layer 104 needs to have a thickness of 10 μm or more.
[0032] The radiation imaging panel 100 can be produced by laminating a protective layer 110, which includes a resin layer 104 having a desired thickness and in which a desired concentration of metal oxide particles 106 is dispersed, formed on a base 201, on top of a scintillator 108.
[0033] For example, the formed protective layer 110 is cut out to match the size of the scintillator 108 of the substrate 101, and then set in a vacuum thermal transfer device. The substrate 101 on which the scintillator 108 has been formed is set in the vacuum thermal transfer device so as to face the protective layer 110. After aligning the base 201 and the substrate 101 using an alignment mark, the substrate 101 and the protective layer 110 are first brought into contact with each other at 30° C., and then heated to 30° C. -1 The pressure is reduced to 10 Pa to remove air bubbles. Furthermore, both substrate 101 and protective layer 110 are heated to 70-100° C. under pressure and held for an appropriate period of time, whereby substrate 101 on which scintillator 108 has been formed and protective layer 110 are bonded together.
[0034] Next, the substrate 101 with the protective layer 110 attached thereto has a connection terminal portion (not shown) connected to a drive substrate and the like via an anisotropic conductive film or the like. Furthermore, a sheet for reinforcing strength is attached to the side of the substrate 101 opposite to the scintillator 108, thereby obtaining the radiation imaging panel 100 of this embodiment.
[0035] Next, the relationship between the concentration of the metal oxide particles 106 of the radiation imaging panel 100, the thickness of the resin layer 104, and the MTF will be described. FIGS. 3 and 4 are diagrams showing the characteristics of the radiation imaging panel 100 produced by changing the concentration of the metal oxide particles 106 and the thickness of the resin layer 104. The characteristics of the radiation imaging panel 100 were evaluated by setting the radiation imaging panel 100 in a drive system, irradiating it with X-rays conforming to the international standard radiation quality RQA5, and measuring the MTF and DQE (Detective Quantum Efficiency). The measurement results of the MTF value and the DQE value at 2 lp / mm for the volume ratio of the metal oxide particles 106 in the resin layer 104 and the thickness t of the resin layer 104 are shown in a list in FIG. 3 and as a graph plotted in FIG. 4. The thickness t of the resin layer 104 is shown as a range after observing multiple SEM images because the height of the phosphor actually varies depending on the column.
[0036] Here, the thickness t of the resin layer 104 is the thickness from the top of each of the columnar crystals 102 in the resin layer 104 to the upper surface of the resin layer 104, as shown in FIG. 1(b). The top of the columnar crystal 102 may be the part of each of the columnar crystals 102 that is the furthest from the substrate 101. The thickness t of the resin layer 104 can be measured by cutting out a small piece after producing the radiation imaging panel 100, exposing the cross section cut by a chemical polishing device, and taking an SEM image. FIG. 5 shows an SEM image of the columnar crystals 102 of the scintillator 108 and the resin layer 104 of the protective layer 110. The thickness t of the resin layer 104 can be controlled by the thickness of the resin 103 when forming the protective layer 110, the heating temperature in the vacuum thermal transfer device, and the maintenance time.
[0037] 3 and 4, it can be seen that when the thickness t of the resin layer 104 is less than 30 μm, the tendency for the MTF to improve changes with the volume ratio of the metal oxide particles 106. Furthermore, it can be seen that when the thickness of the resin layer 104 is less than 30 μm and the concentration of the metal oxide particles 106 in the resin layer 104 is 0.15 vol% or more and less than 7.5 vol%, a higher MTF is exhibited. Furthermore, it can be seen from FIG. 3 that within the range of the thickness of the resin layer 104 and the concentration of the metal oxide particles 106 produced, the DQE value is almost unaffected by either the thickness of the resin layer 104 or the concentration of the metal oxide particles 106.
[0038] For these reasons, the thickness t from the top of each of the columnar crystals 102 in the resin layer 104 to the upper surface of the resin layer 104 is set to 10 μm or more and less than 30 μm, and the concentration of the metal oxide particles 106 in the resin layer 104 is set to 0.15 vol% or more and less than 7.5 vol%. This makes it possible to improve the MTF characteristics in the radiation imaging panel 100 while maintaining the DQE characteristics.
[0039] In the above embodiment, the case where the hot melt resin is used as the resin 103 used in the resin layer 104 has been described, but the resin 103 is not limited to the hot melt resin. For example, the resin 103 used in the resin layer 104 may be a resin having a pressure-sensitive adhesive action due to intermolecular forces, a so-called adhesive material. In this case, the resin 103 may be a material having a lower refractive index than the scintillator 108. For example, the resin 103 may contain at least one of a urethane resin (n: 1.49) and an acrylic resin (n: 1.49 to 1.53). That is, for example, the refractive index of the resin 103 may be 1.49 or more and 1.53 or less. For example, the resin 103 may be a polymethyl methacrylate resin (n: 1.491) out of acrylic resins.
[0040] 6 and 7 are diagrams showing the characteristics of radiation imaging panels 100 produced by changing the concentration of the metal oxide particles 106 and the thickness of the resin layer 104, as in the above-mentioned FIGS. 3 and 4. The radiation imaging panel 100 shown in FIGS. 6 and 7 is similar to the above-mentioned radiation imaging panel 100, except that an acrylic resin is used for the resin 103 instead of a hot melt resin. When an acrylic resin is used for the resin 103, for example, a roll laminator is used to transfer the resin layer 104 onto the base 201 on which the metal layer 202 is formed, thereby forming the protective layer 110. Alternatively, a roll laminator is used to bond the protective layer 110 onto the scintillator 108 on the substrate 101, and a pressure degassing process is performed to produce the radiation imaging panel 100.
[0041] 6 and 7, even when an acrylic resin is used for the resin 103, when the thickness t of the resin layer 104 is less than 30 μm, the tendency of the MTF improving with respect to the volume ratio of the metal oxide particles 106 changes. Furthermore, when the thickness of the resin layer 104 is less than 30 μm and the concentration of the metal oxide particles 106 in the resin layer 104 is 0.15 vol% or more and less than 7.5 vol%, a higher MTF is exhibited. Also, from FIG. 6, it is understood that within the range of the thickness of the resin layer 104 and the concentration of the metal oxide particles 106 produced, the DQE value is almost unaffected by either the thickness of the resin layer 104 or the concentration of the metal oxide particles 106.
[0042] In this way, the thickness t from the top of each of the plurality of columnar crystals 102 in the resin layer 104 to the upper surface of the resin layer 104 is 10 μm or more and less than 30 μm, and the concentration of the metal oxide particles 106 in the resin layer 104 is 0.15 vol% or more and less than 7.5 vol%. This makes it possible to improve the MTF characteristics in the radiation imaging panel 100 while maintaining the DQE characteristics.
[0043] In this embodiment, rutile titanium dioxide particles are used as the metal oxide particles 106. However, even if the above-mentioned metal oxides (e.g., white lead, zinc oxide, yttrium oxide, zirconium oxide) are used, by setting the concentration of the metal oxide particles 106 and the thickness of the resin layer 104 as described above, it is possible to achieve improved MTF characteristics while maintaining the DQE characteristics in the radiation imaging panel 100.
[0044] In addition, in the present embodiment, a case has been described in which the substrate 101 having the pixel region 105 in which a plurality of pixels are arranged is used, but the present invention is not limited to this. For example, the substrate 101 may not have the pixel region 105. In this case, the reference numeral 100 may be called a scintillator plate. For example, by mounting this scintillator plate on a sensor substrate having a pixel region in which a plurality of pixels are arranged, the substrate 101 may function as a radiation imaging panel. Therefore, when the substrate 101 does not have the pixel region 105, the substrate 101 may be a transparent substrate that transmits light emitted by the scintillator 108.
[0045] Hereinafter, a radiation imaging device incorporating the above-mentioned radiation imaging panel 100 and a radiation imaging system 800 using the radiation imaging device incorporating the radiation imaging panel 100 will be described with reference to FIG.
[0046] The radiation imaging system 800 is configured to electrically capture an optical image formed by radiation and obtain an electrical radiation image (i.e., radiation image data). The radiation imaging system 800 includes, for example, a radiation imaging device 801, an exposure control unit 802, a radiation source 803, and a computer 804.
[0047] A radiation source 803 for irradiating radiation to a radiation imaging device 801 starts irradiating radiation in accordance with an exposure command from an exposure control unit 802. The radiation emitted from the radiation source 803 passes through a subject (not shown) and is irradiated to the radiation imaging device 801. The radiation source 803 stops emitting radiation in accordance with a stop command from the exposure control unit 802.
[0048] The radiation imaging apparatus 801 includes the above-mentioned radiation imaging panel 100, a control unit 805 for controlling the radiation imaging panel 100, and a signal processing unit 806 for processing a signal output from the radiation imaging panel 100. The signal processing unit 806 may, for example, perform A / D conversion of the signal output from the radiation imaging panel 100 and output the signal as radiation image data to a computer 804. The signal processing unit 806 may also generate a stop signal for stopping the irradiation of radiation from the radiation source 803 based on the signal output from the radiation imaging panel 100. The stop signal is supplied to the exposure control unit 802 via the computer 804, and the exposure control unit 802 sends a stop command to the radiation source 803 in response to the stop signal.
[0049] The control unit 805 can be configured, for example, by a PLD (Programmable Logic Device) such as an FPGA (Field Programmable Gate Array), or an ASIC (Application Specific Integrated Circuit), or a general-purpose computer with a built-in program, or a combination of all or part of these.
[0050] In addition, in the present embodiment, the signal processing unit 806 is shown as being disposed in the control unit 805 or as a part of the function of the control unit 805, but is not limited thereto. The control unit 805 and the signal processing unit 806 may each have a different configuration. Furthermore, the signal processing unit 806 may be disposed separately from the radiation imaging device 801. For example, the computer 804 may have the function of the signal processing unit 806. For this reason, the signal processing unit 806 may be included in the radiation imaging system 800 as a signal processing device that processes a signal output from the radiation imaging device 801.
[0051] The computer 804 can control the radiation imaging apparatus 801 and the exposure control unit 802, receive radiation image data from the radiation imaging apparatus 801, and perform processing for displaying the data as a radiation image. The computer 804 can also function as an input unit for a user to input conditions for capturing a radiation image.
[0052] As an example, the exposure control unit 802 has an exposure switch, and when the exposure switch is turned on by the user, it sends an exposure command to the radiation source 803 and also sends a start notification indicating the start of radiation emission to the computer 804. In response to the start notification, the computer 804 notifies the control unit 805 of the radiation imaging device 801 of the start of radiation irradiation. In response to this, the control unit 805 causes the radiation imaging panel 100 to generate a signal corresponding to the incident radiation.
[0053] The invention is not limited to the above-described embodiments, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are appended to apprise the public of the scope of the invention. [Explanation of symbols]
[0054] 100: radiation imaging panel, 101: substrate, 102: columnar crystals, 103: resin, 104: resin layer, 106: particles, 108: scintillator, 110: protective layer
Claims
1. A radiation imaging panel including a substrate on which a plurality of pixels, each of which includes a photoelectric conversion element, is disposed, a scintillator disposed on the substrate, and a protective layer disposed so as to cover the scintillator, the scintillator includes a plurality of columnar crystals including an alkali metal halide compound; the protective layer comprises a resin layer containing a resin to which metal oxide particles have been added, a base disposed on a side of the resin layer opposite to the scintillator, and a metal layer disposed between the resin layer and the base, The resin includes a hot melt resin, a thickness from the top of each of the plurality of columnar crystals in the resin layer to an upper surface of the resin layer is 10 μm or more and less than 30 μm; 13. A radiation imaging panel, comprising: a particle concentration in the resin layer of the radiation imaging panel, the particle concentration being equal to or greater than 0.15 vol % and less than 7.5 vol %.
2. 2. The radiation imaging panel according to claim 1, wherein the average particle size of the particles is 200 nm or more and 500 nm or less.
3. 3. The radiation imaging panel according to claim 1, wherein the particles have a refractive index of 1.94 or more and 2.72 or less.
4. 4. The radiation imaging panel according to claim 1, wherein the particles contain at least one of white lead, zinc oxide, and titanium oxide.
5. 5. The radiation imaging panel according to claim 1, wherein the particles contain rutile titanium dioxide.
6. 6. The radiation imaging panel according to claim 1, wherein the alkali metal halide compound contains cesium iodide.
7. A radiation imaging panel as described in any one of claims 1 to 6, characterized in that the concentration of the particles in the resin layer is 0.15 vol% or more and 4.5 vol% or less.
8. A radiation imaging panel according to claim 1 , a control unit for controlling the radiation imaging panel; 13. A radiation imaging apparatus comprising:
9. The radiation imaging apparatus according to claim 8 , a signal processing device for processing a signal output from the radiation imaging device; 1. A radiation imaging system comprising:
10. A scintillator plate including a substrate, a scintillator disposed on the substrate, and a protective layer disposed to cover the scintillator, the scintillator includes a plurality of columnar crystals including an alkali metal halide compound; the protective layer comprises a resin layer containing a resin to which metal oxide particles have been added, a base disposed on a side of the resin layer opposite to the scintillator, and a metal layer disposed between the resin layer and the base, The resin includes a hot melt resin, a thickness from the top of each of the plurality of columnar crystals in the resin layer to an upper surface of the resin layer is 10 μm or more and less than 30 μm; A scintillator plate, characterized in that the concentration of the particles in the resin layer is 0.15 vol % or more and less than 7.5 vol %.
11. 11. The scintillator plate according to claim 10, wherein the substrate is a transparent substrate that transmits light emitted by the scintillator.
12. A scintillator plate as described in claim 10 or 11, characterized in that the concentration of the particles in the resin layer is 0.15 vol% or more and 4.5 vol% or less.
Citation Information
Patent Citations
Radiation detection device
JP2006052980A
Evaporation substrate and scintillator panel
JP2014167405A
Indirect X-ray Imager Having Semi-Transparent layers
US20120181436A1
Scintillator plate, radiation detector and radiation detection system
WO2020129428A1