Porous biomimetic scaffolds, biomedical implants and uses thereof
By aligning fibers and creating channels within scaffolds through controlled cooling of fiber-forming solutions, the method addresses the challenge of replicating natural ECM structures, improving cell support and tissue regeneration.
Patent Information
- Application Number
- JP2023038285
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-06-19
- Filing Date
- 2023-03-13
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2038-06-14
AI Technical Summary
Current biomaterials for tissue engineering struggle to replicate the 3D structure and functionality of natural extracellular matrices, particularly in creating aligned nanofiber-based scaffolds with interconnected macropores that mimic anisotropic tissues, leading to inadequate cell support and limited porosity.
A method involving controlled cooling of fiber-forming molecule solutions to induce solvent crystallization and alignment, forming scaffolds with aligned fibers and channels that mimic the natural ECM, using techniques such as freeze-drying and solvent crystallization to create hierarchical structures with co-aligned nanofibers and macrochannels.
The resulting scaffolds promote cell adhesion, proliferation, and differentiation by providing a biomimetic environment that supports three-dimensional cell culture and tissue regeneration, enhancing nutrient transport and intercellular communication.
Smart Images

Figure 0007565399000001 
Figure 0007565399000002 
Figure 0007565399000003
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to Australian Provisional Patent Application No. 2017902326, filed June 19, 2017, the contents of which are understood to be incorporated by reference.
[0002] The present invention relates to biomaterials and methods for their manufacture for use in tissue engineering applications such as cell culture, tissue regeneration and wound repair. The present invention provides a scaffold that mimics the natural extracellular matrix for use in tissue engineering, as well as a method for preparing and using said scaffold, preferably with fibers and porosity for cell growth. In particular, the method uses a facile strategy to create hierarchical 3D structures with co-aligned nanofibers and optionally macrochannels by manipulating ice crystallization in macromolecular solutions. The present invention also provides the use of the scaffold in promoting cell growth, and as a biomedical implant. [Background technology]
[0003] In tissue engineering, biomaterials have attracted great interest. An ideal biomaterial should be able to provide a biomimetic three-dimensional (3D) environment and support as well as to guide cell behavior and function by interacting with cells as well as by mediating complex multicellular interactions in space and time. To optimally control cell fate and activity, biomaterials that mimic the structural features and functions of the natural extracellular matrix (ECM) are continuously being developed. The natural ECM exists as a complex 3D porous structure of nanofibers with diameters ranging from 50 to 500 nm. The main component of the ECM is collagen, which has various structural arrangements, such as the orientation of collagen fibers in various tissues. In a particular tissue, cells respond perfectly to the features of the ECM to maintain their unique behavior and function.
[0004] In many tissues with anisotropic structural properties (such as dura mater, tendons, ligaments, tympanic membrane and muscle tissues), cells and ECM fibers are highly aligned. These unique alignments support the specific physiological functions of tissues and organs. For example, the radially aligned nanofiber matrix of dura mater and tympanic membrane tissues transport blood and conduct sound, respectively. In skeletal muscle, tendon and ligament tissues, longitudinally aligned fiber bundles support movement and mechanical loading. In two-dimensional (2D) materials, structures with aligned nanofibers have been fabricated using various techniques such as electrospinning and rotary jet spinning. However, these 2D aligned matrices do not mimic the 3D properties of native anisotropic tissues and do not provide support to cells and tissues in 3D space. Furthermore, a drawback of 2D aligned materials is that they have very small pore sizes and low porosity due to mechanical stretching during the fabrication process.
[0005] Aligned fiber-based 3D scaffolds, especially those with interconnected macropores, are extremely difficult to achieve. Moreover, it is difficult to obtain the desired alignment of fibers spatially using currently available techniques (e.g., tubes with short-axis aligned fibers or spheres with centrally aligned fibers). Currently, the main forms of aligned fiber-based structures are two-dimensional membranes and tubes with very thin walls (2D) composed of nanofibers aligned along the long axis of the tube. Moreover, existing 3D scaffolds with random fiber orientation have poor interconnectivity and pore size.
[0006] An ideal material for regenerating anisotropic tissue should have a 3D biomimetic structure with aligned nanofibers and interconnected macropores to guide cell proliferation and facilitate nutrient / oxygen / waste transport / exchange and intercellular communication. Although there is growing interest in mimicking the native structural features and functions of ECM, the preparation of scaffolds with highly aligned nanofibers and large pores remains challenging.
[0007] Currently, the standard treatment for wounds or damaged tissue is to use autografts. However, the use of autografts is often limited due to the high risk of infection and insufficient donor sites. Furthermore, autografts can result in secondary wounds at the donor site, which can cause severe scarring at both the application site and the donor site.
[0008] It is therefore desirable to develop scaffolds with aligned fibers and sufficient interconnectivity and pore size to be suitable materials for use in tissue engineering, as well as methods for preparing and using said scaffolds to promote cell proliferation and tissue formation in bulk 3D scaffolds.
[0009] Discussions of documents, acts, materials, devices, articles and the like are included in this specification solely for the purpose of providing a context for the present invention. No suggestion or implied that any or all of these matters form part of the prior art body or were common general knowledge in the art relevant to this invention by virtue of existing prior to the priority date of each claim of this application.
[0010] When the terms "comprise", "comprises", "comprised" or "comprising" are used in this specification (including the claims), these terms are to be interpreted as specifying the presence of stated features, integers, steps or components, but not as excluding the presence of one or more other features, integers, steps or components or groups thereof. Summary of the Invention [Problem to be solved by the invention]
[0011] The continuing evolution of scaffolds for tissue engineering has been driven by the desire to recapitulate the structural features and functions of the native extracellular matrix (ECM). However, creating 3D structures with aligned nanofibers and interconnected macropores to mimic the ECM of anisotropic tissues remains a challenge. [Means for solving the problem]
[0012] Thus, in one aspect of the invention, there is provided a method of preparing a scaffold, said method comprising the steps of providing a solution comprising fiber-forming molecules, exposing the solution to a cooling medium to establish a temperature differential at an interface between the cooling medium and the solution, and cooling the solution as a result of the temperature differential to induce solvent crystallization and fiber alignment in the solution to create the scaffold.
[0013] Advantageously, in certain embodiments, the scaffolds of the invention having aligned fibers can promote at least one of cell adhesion, proliferation and differentiation because the scaffold mimics the structure of the natural extracellular matrix.
[0014] Thus, in a further embodiment, the invention further comprises exposing the scaffold to the solution followed by an additional cooling step to induce solvent crystallization and channels within the scaffold, hi certain embodiments, the channels are substantially co-aligned with the aligned fibers.
[0015] In certain embodiments, the channels formed in the scaffold can promote at least one of cell adhesion (trapping) and proliferation. The channels formed in the scaffold of the present invention can promote three-dimensional cell growth or cell culture for tissue regeneration.
[0016] Thus, in another aspect, the present invention provides a porous biomimetic scaffold comprising a matrix of substantially aligned fibers. In yet another aspect, the present invention provides a porous biomimetic scaffold comprising a three-dimensional matrix of substantially aligned fibers. In yet another aspect, the present invention provides a porous biomimetic scaffold comprising a matrix of fibers. In some embodiments, the fibers are aligned. In some embodiments, the fibers are radially aligned fibers, linearly aligned fibers, or longitudinally aligned fibers. In some embodiments, the fibers are aligned in one direction.
[0017] The scaffolds of the present invention can be used for cell culture and tissue engineering applications. In certain embodiments, the scaffolds provided by the present invention include a method of treating a mammal suffering from tissue damage and in need of tissue repair and / or regeneration, the method comprising applying the scaffolds of the present invention to the site of injury.
[0018] In some embodiments, the inventors have discovered that the scaffolds are stable in biological systems under certain circumstances and therefore can be used for cell culture, drug delivery, wound healing, or treatment of damaged tissue. [Brief description of the drawings]
[0019] [Figure 1] (a) Scaffold with radially aligned nanofibers and macrochannels. The channel walls are composed of nanofibers aligned along the long axis of the channel, as well as pores and particles. (b) Scaffold with vertically aligned nanofibers and macrochannels. [Diagram 2] Fabrication of 3D silk fibroin (SF) scaffolds (A(F&C) scaffolds) with radially co-aligned nanofibers and macrochannels by a simple freeze-drying technique. The hole (in 4.A(F&C) scaffold above) is a top view of the central channel of A(F&C) scaffold. AFb: aligned nanofiber scaffolds, AF: water-resistant aligned nanofiber scaffolds without macrochannels, and A(F&C): water-resistant scaffolds with radially co-aligned nanofibers and macrochannels. [Diagram 3] Hierarchical structure of 3D scaffolds (A(F&C)) with radially aligned nanofibers and channels. (a) Micro-CT image showing the radially aligned channel structure of the scaffold. Scale bar: 1000 μm. (b) SEM images of the channel wall at various magnifications revealing the aligned nanofiber structure with nanoparticles and pores. (Large arrows indicate the orientation of aligned nanofibers. Particles, pores and aligned nanofibers on the channel wall are indicated by small arrows, respectively. Scale bars: 10, 2 and 1 μm from left to right, respectively. (c) Schematic dimensional representation of the relevant structures. [Figure 4] Polypropylene porous microfiber materials modified with locally aligned silk fibroin (SF) nanofibers of the present invention (0.0125%, 0.025% and 0.05% (w / v) silk fibroin solutions were used for nanofibers in a, b and c, respectively). a', b' and c' are enlarged views of a, b and c, respectively. Scale bars: a, b and c, 200 μm; a' and b', 10 μm; c', 30 μm. [Diagram 5] Polypropylene porous microfibrillar materials modified with locally aligned alginate nanofibers using 0.025% (w / v) alginate solution (a, b, c; a, b and c are at different magnifications) and locally aligned gelatin nanofibers using 0.025% (w / v) gelatin solution of the present invention (d, e, f; d, e and f are at different magnifications). Scale bars: a, b, c, d, e and f are 100, 10, 1, 200, 20 and 1 μm, respectively. [Figure 6] 3D A(F&C) scaffolds enhance the capture and proliferation of adherent human umbilical vein endothelial cells (HUVECs) and guide cell migration and proliferation through aligned nanofibers and channels. (a) Viability (MTS extinction coefficient) of HUVECs captured by 3D AF, W, W&F and A(F&C) scaffolds. (b) Viability (MTS extinction coefficient) of HUVECs on 3D AF, W, W&F and A(F&C) scaffolds after different culture periods. (c) Scheme showing how to read the images shown in d. (d) Proliferation of HUVECs on 3D AF, W, W&F and A(F&C) scaffolds after 3 days of culture. Scale bars: 25 μm for W, W&F, AF and inset 1; 75 μm for A(F&C). [Figure 7]The aligned nanofibers and channels in the 3D A(F&C) scaffolds promote the formation of CD31-positive vessel-like structures by inducing the proliferation, migration and interaction of adherent HUVECs after 21 days of culture (Figure 6c shows how to read the images shown in Figure 7). (a) HUVEC proliferation and interaction in 3D A(F&C), AF, W&F and W scaffolds. Scale bars: 50 μm for A(F&C), W&F and W; 25 μm for AF. (b) Sequential confocal slices of the channels in A(F&C) shown in (a). Scale bars: 50 μm. [Figure 8] Aligned nanofibers and channels in 3D A(F&C) scaffolds promote capture of non-adherent Embryonic Dorsal Root Ganglion Neuron cells (DRG) and induce 3D outgrowth of DRG neurites. (a) Viability (MTS extinction coefficient) of DRG captured by 3D AF, W, W&F and A(F&C) scaffolds. (b) Confocal fluorescence microscopy images revealing that the structure of W, W&F and AF scaffolds restricts DRG and DRG neurites from growing on the surface of the scaffolds. Scale bars: 100 μm for W and W&F scaffolds; 50 μm for AF scaffolds. (c) In 3D A(F&C) scaffolds, aligned nanofibers and channels induce 3D outgrowth of DRG neurites. Scale bars: 75, 25 and 25 μm from left to right, respectively. [Figure 9]The 3D A(F&C) scaffold induces the proliferation, migration and interaction of both adherent HUVECs and non-adherent DRG and DRG neurites with radially aligned channels and nanofibers. Adherent HUVECs are mainly guided by aligned nanofibers, whereas non-adherent DRG and DRG neurites are mainly guided by aligned channels. (a) HUVECs proliferating and interacting along aligned nanofibers on the channel wall. (b) HUVECs assemble into CD31-positive vessel-like structures along aligned nanofibers on the channel wall. (c), (d) and (e) DRG and DRG neurites proliferating along aligned channels, suggesting 3D proliferation of DRG and DRG neurites in the A(F&C) scaffold. All scale bars are 25 μm. [Figure 10] (a) Representative SEM image showing aligned nanofibers and nanoparticles within the AFb scaffold. The fast Fourier transform (FFT) pattern in the inset suggests that these nanofibers were well aligned in the radial direction. Scale bars: 2, 1 and 10 μm from left to right, respectively. (b) Directional freezing of silk fibroin aqueous solutions in liquid nitrogen allows the fabrication of 3D silk fibroin nanofiber scaffolds with various shapes (including cylinders, tubes and particles or spheres), diameters and thicknesses as well as various nanofiber alignments. [Figure 11] Effect of freezing temperature on the morphological structure of 3D silk fibroin scaffolds. (a) SEM images reveal that silk fibroin aqueous solution frozen at -80°C results in 3D scaffolds (W&Fb) with a hybrid structure with short channels / pores / fibers. Scale bars: 200, 30 and 100 μm from left to right, respectively. (b) SEM images show that silk fibroin aqueous solution frozen at -20°C produces 3D scaffolds (Wb) with a wall-like porous structure. Scale bars: 200, 20 and 100 μm from left to right, respectively. [Figure 12]Representative images of A(F&C) scaffolds obtained from a SF / gelatin mixture (a), sodium alginate (b). Red arrows indicate channels within the scaffold with aligned nanofibers on the channel walls. Scale bars: a, 20 μm; b and c, 2 μm. [Figure 13] Micro-CT images of the hybrid structure (containing short channels / pores / nanofibers) of W&F and the wall-like porous structure of W 3D scaffolds. The structural details are clearly shown in Figure 14. Scale bars are both 1000 μm. [Figure 14] (a) SEM image of water-resistant W&F scaffolds after post-treatment. Scale bars: 100, 20, and 100 μm from left to right, respectively. (b) SEM image of water-resistant W scaffolds after post-treatment. Scale bars: 100, 20, and 100 μm from left to right, respectively. [Figure 15] ATR-FTIR spectra of 3D silk fibroin scaffolds. (a) ATR-FTIR spectra of silk fibroin scaffolds obtained from different freezing temperatures, i.e., -20 °C (Wb), -80 °C (W&Fb) and liquid nitrogen (AFb). (b) ATR-FTIR spectra of post-treated silk fibroin scaffolds. All scaffolds (A(F&C), W&F and W) show peaks at approximately 1517, 1622 and 1700 cm-1, suggesting that the structure of silk fibroin transitioned from random coil to β-sheet upon post-treatment. [Figure 16] (a) Compressive modulus of 3D W, W&F and A(F&C) silk fibroin scaffolds. (b) Morphology of scaffolds after mechanical testing. It is noteworthy that after being compressed in mechanical testing, A(F&C) scaffold still maintains good radially aligned morphology and structure, while the surface of the scaffold shows slight collapse, possibly due to the damage of some channels. [Figure 17] Proliferation of DRGs on W and W&F scaffolds after 21 days of culture. The expansion and outgrowth of DRG neurites on W and W&F scaffolds is blocked by the surrounding material, suggesting that the scaffolds do not provide a favorable 3D environment for DRGs. Scale bars: 100 and 25 μm for W and W&F, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The continuing evolution of scaffolds for tissue engineering has been driven by the desire to recapitulate the structural features and functions of the native extracellular matrix (ECM). However, creating scaffolds with aligned nanofibers and interconnecting macropores to mimic the ECM of anisotropic tissues remains a challenge, particularly in the development of 3D scaffolds.
[0021] (Scaffolds with Aligned Fibers) Thus, in one aspect of the invention, there is provided a method of preparing a scaffold, said method comprising the steps of providing a solution comprising fiber-forming molecules, exposing the solution to a cooling medium to establish a temperature differential at an interface between the cooling medium and the solution, and cooling the solution as a result of the temperature differential to induce solvent crystallization and fiber alignment in the solution to create the scaffold.
[0022] The inventors have discovered that controlled cooling of a solution containing fiber-forming molecules induces solvent crystallization in which fibers can align to create scaffolds. Fiber alignment can be directionally controlled such that sophisticated scaffolds can be produced with fibers aligned in the direction in which the solvent crystallization forms.
[0023] The method of the present invention, as used herein, can be preferably used to prepare any "scaffold", which refers to a three-dimensional matrix of fibers suitable as a template for cell carriers for cell culture, tissue repair, tissue engineering or related applications. Preferably, the scaffold is a 3D scaffold that contains channels and pores that allow and facilitate cell culture and the flow of biochemical and physicochemical factors within the scaffold necessary for cell culture and survival.
[0024] The scaffold is formed from a solution containing fiber-forming molecules. The technique used to prepare the scaffold according to the method of the present invention depends on the solution, fiber-forming molecules and cooling medium used. It will also be understood that the technique used will affect the direction of fiber alignment, whether the fibers are aligned vertically or radially. The solution can be directly or indirectly exposed to the cooling medium to establish a temperature difference at the interface between the solution and the cooling medium. In certain embodiments, the solution containing fiber-forming molecules is previously contained in a container and indirectly exposed to the solution for cooling.
[0025] Alternatively, in some embodiments, the container may be immersed in a cooling medium, followed by adding a solution containing fiber-forming molecules to the container to induce fiber alignment. Any suitable container material may be used in the present invention, provided that a temperature difference is established at the interface between the solution and the cooling medium. In some embodiments, the container material is selected from, but not limited to, glass, metal, plastic, ceramic, or a combination thereof.
[0026] In certain embodiments, the solution containing the fiber-forming molecules can be directly exposed to the cooling medium, for example, the solution containing the fiber-forming molecules can be dripped, sprayed, or injected directly into the cooling medium to establish a temperature differential at the interface between the cooling medium and the solution to induce solvent crystallization and fiber alignment within the scaffold.
[0027] Without wishing to be bound by any theory, the inventors believe that the alignment of the fibers is controlled by solvent crystallization, which occurs when the temperature difference between the solution and the cooling medium is sufficient to form crystal nuclei. For example, if the solvent is water, ice nuclei will form if the temperature difference is sufficient to cause freezing, and the ice crystals so formed will radiate into the solution from the interface between the solution and the cooling medium. The solvent crystals and the direction in which they form are believed to act as templates to control the alignment direction of the fibers.
[0028] The temperature difference is essential for the formation of solvent crystallization and alignment of the fibers and is determined by the temperature difference between the solution and the cooling medium.
[0029] In certain embodiments, the temperature difference is sufficient to promote nucleation of solvent crystals at the interface. The temperature difference can be measured relative to the solution. For example, if the solution has a temperature of 20° C. and the cooling medium has a temperature of −40° C., the temperature difference will be −60° C. relative to the solution. In certain embodiments, the temperature difference is at least −120° C. relative to the solution. In certain embodiments, the temperature difference is at least −196° C. relative to the solution. In certain embodiments, the temperature difference is in the range of −20° C. to −296° C. relative to the solution. In certain embodiments, the temperature difference is in the range of −80° C. to −296° C. relative to the solution, or −180° C. to −296° C. relative to the solution. In certain embodiments, the temperature difference is in the range of −120° C. to −296° C. relative to the solution. In certain embodiments, the temperature difference is in the range of −20° C. to −196° C. relative to the solution, or −30° C., −40° C., −50° C., −60° C., or −70° C. relative to the solution. In certain embodiments, the temperature difference is in the range of -80°C to -196°C for the solution, or -90°C or -100°C for the solution. In certain embodiments, the temperature difference is in the range of -100°C to -196°C for the solution, or -110°C for the solution. In certain embodiments, the temperature difference is in the range of -120°C to -196°C for the solution, or -130°C, -140°C, -150°C for the solution. In certain embodiments, the temperature difference is in the range of -150°C to -196°C for the solution, or -160°C for the solution. In certain embodiments, the temperature difference is in the range of -170°C to -196°C for the solution, or -180°C or -190°C for the solution.
[0030] The direction of fiber alignment can be controlled by adjusting the direction of the temperature difference (i.e., cooling direction). In some embodiments, the establishment of a temperature difference between the cooling medium and the solution containing fiber-forming molecules induces aligned fibers from the interface between the solution and the cooling medium. In some embodiments, the establishment of a temperature difference between the cooling medium and the solution containing fiber-forming molecules induces unidirectionally aligned fibers from the interface between the solution and the cooling medium. As used herein, the term "unidirectionally aligned fibers" refers to fibers in a scaffold that are oriented in a single direction. Non-limiting examples of unidirectionally aligned fibers include fibers that are approximately parallel to each other (linearly aligned) or fibers that extend approximately toward a point in space (radially aligned). It should be understood that not all fibers must be oriented in a single direction, and some deviation in direction is contemplated.
[0031] In certain embodiments, a temperature differential is established circumferentially relative to the solution to induce radially aligned fibers within the scaffold. In certain embodiments, a temperature differential is established along the plane of the interface to induce linear or longitudinally aligned fibers within the scaffold. Thus, the plane can be parallel or perpendicular to the interface.
[0032] As will be appreciated by those skilled in the relevant art, the temperature difference is a relative measure of the temperature range between the cooling medium and the solution containing the fiber-forming molecules. It may also be convenient to express the temperature sufficient to induce fiber alignment in absolute terms. For example, it may represent the temperature of the cooling medium to induce nucleation of solvent crystals for fiber alignment.
[0033] In some embodiments, the cooling medium is at a temperature less than -196°C. In some embodiments, the cooling medium is at a temperature between -80°C and -196°C. In some embodiments, the cooling medium is at a temperature between -80°C or -90°C, less than -100°C. In some embodiments, the cooling medium is at a temperature between -100°C and -196°C or between -110°C and -196°C. In some embodiments, the cooling medium is at a temperature between -120°C and -196°C or between -130°C and -196°C. In some embodiments, the cooling medium is at a temperature between -140°C and -196°C or between -150°C and -196°C. In some embodiments, the cooling medium is at a temperature between -160°C and -196°C, or between -170°C and -196°C, or between -180°C and -196°C.
[0034] Those skilled in the relevant art will also appreciate that the cooling rate of the solution containing the fiber-forming molecules can affect the alignment of the fibers. In some embodiments, the solution is cooled at a rate of 0.2° C.s -1 ~260℃.s -1 In some embodiments, the solution is cooled at a rate of 5° C.s -1 ~260℃.s -1 or 10℃.s -1 ~260℃.s -1 or 15℃.s -1 ~260℃.s -1 In some embodiments, the solution is cooled at a rate of 20° C.s -1 ~260℃.s -1 or 25℃.s -1 ~260℃.s -1 , 30℃.s -1 ~260℃.s -1 , 35℃.s -1 ~260℃.s -1 or 40℃.s -1 ~260℃.s -1 In some embodiments, the solution is cooled at a rate of 50° C.s -1 ~260℃.s -1 or 60℃.s -1 ~260℃.s -1 or 70℃.s -1 ~260℃.s -1In some embodiments, the solution is cooled at a rate of 80° C.s -1 ~260℃.s -1 or 90℃.s -1 ~260℃.s -1 , 100℃.s -1 ~260℃.s -1 or 110℃.s -1 ~260℃.s -1 In some embodiments, the solution is cooled at a rate of 120° C.s -1 ~260℃.s -1 or 130℃.s -1 ~260℃.s -1 or 140℃.s -1 ~260℃.s -1 In some embodiments, the solution is cooled at a rate of 150° C.s -1 ~260℃.s -1 or 160℃.s -1 ~260℃.s -1 , 170℃.s -1 ~260℃.s -1 , 180℃.s -1 ~260℃.s -1 , 190℃.s -1 ~260℃.s -1 , 200℃.s -1 ~260℃.s -1 , 210℃.s -1 ~260℃.s -1 , 220℃.s -1 ~260℃.s -1 , 230℃.s -1 ~260℃.s -1 , 240℃.s -1 ~260℃.s -1 or 250℃.s -1 ~260℃.s -1 The temperature is cooled at a rate of
[0035] In certain embodiments, a sample of a solution containing fiber-forming molecules can be gradually immersed in a cooling medium to induce fiber alignment within the scaffold. In certain embodiments, the solution is gradually immersed in a cooling medium for 1-15 mm.min. -1 In certain embodiments, the solution is immersed in the cooling medium at a rate of 3 to 15 mm.min -1In a particular embodiment, the solution is immersed in the cooling medium at a rate of 1 to 10 mm.min -1 In a particular embodiment, the solution is immersed in the cooling medium at a rate of 5 to 10 mm.min -1 In a particular embodiment, the solution is immersed in the cooling medium at a rate of 5 to 8 mm.min -1 The workpiece is immersed in the cooling medium at a rate of
[0036] In the method of the present invention, any suitable cooling medium can be used to induce fiber alignment within the scaffold. In theory, the cooling medium can be solid, liquid or gas, depending on the exact nature of the cooling medium. For example, the cooling medium can be liquid nitrogen, dry ice, air, liquid ethane, liquid CO2 and combinations thereof. In certain embodiments, the cooling medium is a freezer. In certain embodiments, the cooling medium is dry ice combined with at least one of tetrachloroethylene, carbon tetrachloride, 1,3-dichlorobenzene, o-xylene, m-toluidine, acetonitrile, pyridine, m-xylene, n-octane, isopropyl ether, acetone, butyl acetate, propylamine. In some embodiments, the cooling medium is liquid nitrogen combined with at least one of ethyl acetate, n-butanol, hexane, acetone, toluene, methanol, ethyl ether, cyclohexane, ethanol, ethyl ether, n-pentane, isopentane. Most preferably, the cooling medium is liquid nitrogen.
[0037] A misalignment in the direction of the fiber alignment is envisaged. It may be convenient to express the misalignment of the fibers relative to the surface normal of the interface between the cooling medium and the solution containing the fiber-forming molecules. In one embodiment, the fibers are aligned at 0° to 30° relative to the surface normal of the interface. In one embodiment, the fibers are aligned at 0° to 25° relative to the surface normal of the interface. In one embodiment, the fibers are aligned at 0° to 20° relative to the surface normal of the interface. In one embodiment, the fibers are aligned at 0° to 15° relative to the surface normal of the interface. In one embodiment, the fibers are aligned at 0° to 10° relative to the surface normal of the interface. In one embodiment, the fibers are aligned at 0° to 5° relative to the surface normal of the interface.
[0038] The formation of solvent crystals may act as a template to provide control of fiber alignment within the scaffold. The diameter of the solvent crystals depends on the solvent used, the cooling rate, and the cooling medium used. In the method of the present invention, solvent crystals of any suitable diameter can be used to induce fiber alignment. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 20 nm to 5 mm, 20 nm to 4 mm, 20 nm to 3 mm, 20 nm to 2 mm, or 20 nm to 1 mm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 1 nm to 500 μm, 10 nm to 400 μm, or 10 nm to 300 μm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 10 nm to 200 μm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 10 nm to 100 μm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 10 nm to 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm, 20 μm, or 10 μm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 10 nm to 5 μm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 100 μm to 2 mm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 10 to 3000 nm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 10 to 3000 nm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 20 to 2500 nm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 20 to 2000 nm. In one embodiment, the solvent crystals formed from the solvent crystallization have a diameter of 50 to 2000 nm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 50 to 1500 nm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 50 to 1000 nm. In one embodiment, the solvent crystals formed from solvent crystallization have a diameter of 50 to 700 nm.
[0039] The duration of the cooling step can affect the diameter of the solvent crystals and the resulting fiber diameter. Any suitable duration can be used, as long as it is sufficient to induce fiber alignment within the scaffold. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 10 minutes. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 20 minutes. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 30 minutes. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 1 hour. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 5 minutes. In some embodiments, the solution containing fiber-forming molecules is cooled for less than 1 minute.
[0040] As will be understood by those skilled in the relevant art, the scaffold prepared by the method of the present invention can retain the solvent crystals formed by solvent crystallization. The solvent crystals can be removed from the scaffold using any suitable technique. For example, the scaffold prepared by the method of the present invention can be freeze-dried to remove the solvent crystals. Alternatively, the solvent crystals can be thawed into a solution state after cooling and the solvent can be removed under reduced pressure, such as vacuum or vacuum drying oven. In some embodiments, the solvent crystals can be removed from the scaffold using a desiccator.
[0041] Depending on the fiber-forming molecules used, the scaffold may be water-soluble. In some embodiments, the scaffold may be treated to render it water-resistant. Any suitable agent may be used to treat the scaffold to render it water-resistant. For example, the scaffold may be exposed to the group consisting of ethanol, methanol, genipin, glutaraldehyde, 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide hydrochloride, calcium chloride, water, or combinations thereof. Those skilled in the art will understand that the ethanol, methanol, genipin, glutaraldehyde, 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide hydrochloride, calcium chloride, or water may be in liquid or gas phase (e.g., ethanol solution or ethanol vapor). In certain embodiments, the scaffold is water-resistant.
[0042] In other embodiments, the scaffold can be treated to induce crosslinking between aligned fibers. For example, the scaffold can be exposed to glutaraldehyde or electromagnetic radiation to induce crosslinking within the scaffold. In some embodiments, the scaffold can be exposed to at least one of methanol, ethanol, genipin, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, calcium chloride, water, plasma radiation, or combinations thereof to induce crosslinking within the scaffold. Those skilled in the art will understand that the methanol, ethanol, genipin, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, calcium chloride, or water can be in a liquid phase or a gas phase (e.g., an ethanol solution or ethanol vapor).
[0043] It will be apparent to those skilled in the relevant art that any suitable solvent can be used to dissolve the fiber-forming molecules to form a solution. In one embodiment, the solvent is water, an organic solvent, an inorganic non-aqueous solvent, and combinations thereof. In one embodiment, the solution containing the fiber-forming molecules is an aqueous solution. It will be understood that when the solution is an aqueous solution, the solvent crystals formed from the crystallization are ice crystals.
[0044] Suitable organic solvents may be selected from the group consisting of pentane, cyclopentane, hexane, cyclohexane, benzene, toluene, 1,4-dioxane, chloroform, diethyl ether, dichloromethane, tetrahydrofuran, ethyl acetate, acetone, dimethylformamide, acetonitrile, dimethylsulfoxide, nitromethane, propylene carbonate, n-butanol, isopropanol, n-propanol, ethanol, methanol, formic acid, acetic acid, hexafluoroisopropanol, trifluoroacetic acid, and combinations thereof.
[0045] Suitable inorganic solvents may be selected from the group consisting of liquid ammonia, liquid sulfur dioxide, sulfuryl chloride, sulfuryl chloride fluoride, phosphoryl chloride, dinitrogen tetroxide, antimony trichloride, bromine pentafluoride, hydrogen fluoride, neat sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, boric acid, hydrofluoric acid, hydrobromic acid, perchloric acid, hydroiodic acid, and combinations thereof.
[0046] In certain embodiments, the solution containing the fiber-forming molecules can include a mixture of two or more miscible solvents, such as a mixture of water and an aqueous solvent, a mixture of two or more organic solvents, or a mixture of an organic and an aqueous solvent.
[0047] The amount of fiber-forming molecules dissolved in the solution may be any suitable amount, and one of ordinary skill in the relevant art will understand that the amount dissolved may depend on the solubility of the fiber-forming molecules and the solvent used. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 0.001% to 35% w / v. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 1% to 20% w / v. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 1% to 25% w / v. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 1% to 15% w / v. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 1% to 10% w / v. In certain embodiments, the solution containing the fiber-forming molecules is in an amount of 1% to 5% w / v.
[0048] The present invention also relates to a porous biomimetic scaffold comprising a three-dimensional matrix of substantially aligned fibers. In some embodiments, the fibers are aligned in one direction. In some embodiments, the fibers are aligned radially. In some embodiments, the fibers are aligned linearly or longitudinally.
[0049] The diameter of the fibers in the scaffolds of the invention depends on the solvent, cooling rate, fiber-forming molecules and cooling medium used. In certain embodiments, the diameter of the fibers is 20-5000 nm, 20-4000 nm or 20-3000 nm. In certain embodiments, the diameter of the fibers is 20 to 2500 nm, 2000 nm or 1500 nm. In certain embodiments, the diameter of the fibers is 20-1000 nm. In certain embodiments, the diameter of the fibers is 50-600 nm. In certain embodiments, the diameter of the fibers is 20 to 800 nm. In certain embodiments, the diameter of the fibers is 100-500 nm. In certain embodiments, the diameter of the fibers is 300-800 nm. In certain embodiments, the diameter of the fibers is 300-600 nm.
[0050] It may also be convenient to describe the fibers in terms of the length of the aligned fibers. In certain embodiments, the aligned fibers have a length of at least 50 nm. In certain embodiments, the aligned fibers have a length of 50 nm to 50 mm. In certain embodiments, the aligned fibers have a length of 50 nm to 4 mm. In certain embodiments, the aligned fibers have a length of 50 nm to 2 mm. In certain embodiments, the aligned fibers have a length of 50 nm to 500 μm. In certain embodiments, the aligned fibers have a length of 50 nm to 1000 μm. In certain embodiments, the aligned fibers have a length of 100 nm to 500 μm. In certain embodiments, the aligned fibers have a length of 50 nm to 5000 nm. In certain embodiments, the aligned fibers have a length of 50 nm to 1000 nm. In certain embodiments, the aligned fibers have a length of 100 nm to 500 nm. In certain embodiments, the aligned fibers have a length of 50 nm to 500 nm. In certain embodiments, the aligned fibers have a length between 50 nm and 5 mm. In certain embodiments, the aligned fibers have a length between 50 nm and 10 mm. In certain embodiments, the aligned fibers have a length between 50 nm and 20 mm. In certain embodiments, the aligned fibers have a length between 50 nm and 30 mm. In certain embodiments, the aligned fibers have a length between 50 nm and 40 mm.
[0051] As mentioned above, the scaffold of the present invention is a three-dimensional matrix of fibers suitable for cell culture, tissue repair, tissue engineering or related applications. The scaffold can have pores of any diameter suitable for cell culture, tissue repair, tissue engineering or related applications. In certain embodiments, the scaffold has pores with a diameter of 1 nm to 500 μm or 20 nm to 500 μm. In certain embodiments, the scaffold has pores with a diameter of 20 nm to 400 μm. In certain embodiments, the scaffold has pores with a diameter of 20 nm to 300 μm. In certain embodiments, the scaffold has pores with a diameter of 20 nm to 200 μm. In certain embodiments, the scaffold has pores with a diameter of 20 nm to 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm, 20 μm, 10 μm or 5 μm. In certain embodiments, the scaffold has pores with a diameter of 20 to 1500 nm. In certain embodiments, the scaffold has pores with a diameter of 50 to 1000 nm. In certain embodiments, the scaffold has pores with a diameter of 20 to 800 nm. In certain embodiments, the scaffold has pores with a diameter of 50 to 600 nm. In certain embodiments, the scaffold has pores with a diameter of 100 to 600 nm. In certain embodiments, the scaffold has pores with a diameter of 20 to 600 nm. In certain embodiments, the scaffold has pores with a diameter of 20 to 500 nm.
[0052] The scaffolds of the invention can also be conveniently described in terms of porosity. The porosity of the scaffold may depend on the fiber-forming molecules and solvents used. The porosity of the scaffold was calculated as the ratio of void volume to total sample volume. Thus, in certain embodiments, the scaffold has a porosity of 0.01%-95%. In certain embodiments, the scaffold has a porosity of 20%-95%, 30%-95% or 40%-95%. In certain embodiments, the scaffold has a porosity of 40%-90%, 50%-90%, 60%-90%, 70%-90%, 80%-90% or 85%-90%. In certain embodiments, the scaffold has a porosity of 40%-80%, 40%-70%, 40%-60% or 40%-50%. In certain embodiments, the scaffold has a porosity of 60%-80% or 65%-75%. In certain embodiments, the scaffold has a porosity of 30%-60%, 30%-50% or 30%-40%.
[0053] It will be understood that the amount of aligned fibers within the scaffold may vary. This variation in the amount of aligned fibers within the scaffold can be accounted for based on the total dry weight of the scaffold. Thus, in some embodiments, based on the total dry weight of the scaffold, at least 5% w / w of the scaffold comprises aligned fibers. In some embodiments, based on the total dry weight of the scaffold, at least 10% w / w, 20% w / w, 30% w / w, 40% w / w, 50% w / w or 60% w / w of the scaffold comprises aligned fibers. In some embodiments, based on the total dry weight of the scaffold, at least 70% w / w of the scaffold comprises aligned fibers. In some embodiments, based on the total dry weight of the scaffold, at least 80% w / w of the scaffold comprises aligned fibers. In some embodiments, based on the total dry weight of the scaffold, at least 90% w / w of the scaffold comprises aligned fibers. In some embodiments, based on the total dry weight of the scaffold, the scaffold is comprised of 50%-90% w / w aligned fibers. In some embodiments, the scaffold is comprised of 60%-90% w / w aligned fibers, based on the total dry weight of the scaffold. In some embodiments, the scaffold is comprised of 70%-90% w / w aligned fibers, based on the total dry weight of the scaffold. In some embodiments, the scaffold is comprised of 80%-90% w / w aligned fibers, based on the total dry weight of the scaffold.
[0054] As will be appreciated by those skilled in the relevant art, the scaffold can take any suitable shape, for example, it can be in the shape of a sphere, cube, prism, fiber, rod, tetrahedron, tube or irregularly shaped particle. As will be appreciated by those skilled in the relevant art, the shape of the scaffold can be controlled by using the containers described above, and the shape of the container can typically determine the shape of the scaffold that is ultimately produced.
[0055] Typically, radially aligned fiber scaffolds can be prepared by providing a solution of fiber-forming molecules in a cylindrical sample tube, which can be immersed in a cooling medium (such as liquid nitrogen) to establish a circumferential temperature difference at the interface between the cooling medium and the solution, inducing the formation of radially aligned fibers within the scaffold.
[0056] Alternatively, linear or longitudinally aligned fiber scaffolds can typically be prepared by providing a solution of fiber-forming molecules in a cylindrical sample tube with a flat bottom, which can be slowly lowered from the flat bottom end into a cooling medium (such as liquid nitrogen) to establish a temperature difference at the interface between the cooling medium and the solution along a plane substantially parallel to the bottom, inducing the formation of linear or longitudinally aligned fibers within the scaffold.
[0057] The scaffolds can be of any suitable size, with the size being determined in part by the desired size of the final scaffold produced, or the size of the container, if used. In certain embodiments, the size of the scaffold can be controlled by mechanical processing, such as cutting the scaffold using a blade or laser. In other embodiments, the scaffold is formed by controlling the cooling of a solution containing the fiber-forming molecules, such that once the scaffold is formed, the cooling step is terminated after the desired scaffold size is reached.
[0058] The scaffolds of the invention are typically less than 10 cm in at least one dimension. In one embodiment, the scaffold has a size of 20 nm to 10 cm in at least one dimension. In one embodiment, the scaffold has a size of 1 mm to 10 cm in at least one dimension. In one embodiment, the scaffold has a size of 5 mm to 8 cm in at least one dimension. In one embodiment, the scaffold has a size of 5 mm to 5 cm in at least one dimension. In one embodiment, the scaffold has a size of 1 mm to 3 cm in at least one dimension. In one embodiment, the scaffold has a size of 1 mm to 2 cm in at least one dimension. In one embodiment, the scaffold has a size of 1 mm to 1 cm in at least one dimension.
[0059] In certain embodiments, the scaffold of the present invention has a compressive modulus of 5-5000 kPa. In certain embodiments, the scaffold of the present invention has a compressive modulus of 5 kPa to 4500 kPa, 4000 kPa, 3500 kPa, 3000 kPa, 2500 kPa, 2000 kPa, 1500 kPa, 1000 kPa, 500 kPa, 400 kPa, 300 kPa or 200 kPa. In certain embodiments, the scaffold of the present invention has a compressive modulus of 20-160 kPa. In certain embodiments, the scaffold has a compressive modulus of 20-140 kPa. In certain embodiments, the scaffold has a compressive modulus of 20-120 kPa. In certain embodiments, the scaffold has a compressive modulus of 40-100 kPa. In certain embodiments, the scaffold has a compressive modulus of 60-100 kPa. In certain embodiments, the scaffold has a compressive modulus of 70-100 kPa. In certain embodiments, the scaffold has a compressive modulus of 80-100 kPa.
[0060] Scaffolds with Aligned Fibers and Channels In some embodiments, the methods of the present invention may further comprise exposing the scaffold to a solution or solvent followed by an additional cooling step to induce solvent crystallization and channels within the scaffold. In some embodiments, the channels are substantially co-aligned with the aligned fibers. In some embodiments, the channels may be microchannels or macrochannels.
[0061] It is understood that the additional cooling step can be at any temperature suitable for inducing channels within the scaffold. In one embodiment, the additional cooling step is at a temperature of -5°C to -196°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -196°C. In one embodiment, the additional cooling step is at a temperature of -5°C to -80°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -80°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -60°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -40°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -30°C. In one embodiment, the additional cooling step is at a temperature of -10°C to -25°C, -11°C to -25°C, -12°C to -25°C, -13°C to -25°C, -14°C to -25°C, -15°C to -25°C, -16°C to -25°C, -17°C to -25°C, -18°C to -24°C, -18°C to -23°C, -18°C to -22°C or -19°C to -21°C.
[0062] The inventors believe that the formation of solvent crystals formed from the additional cooling step induces channel formation within the scaffold. Without wishing to be bound by any theory, the inventors believe that the use of high temperatures for the additional cooling step induces large solvent crystals. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 20 nm to 4 mm. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 100 μm to 2 mm. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 50 nm to 1000 nm. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 100 μm to 2 mm. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 100 μm to 1000 μm. In one embodiment, the solvent crystals formed during the additional cooling step have a diameter of 500 μm to 1000 μm.
[0063] As will be appreciated, the duration of the additional cooling step can affect the diameter of the solvent crystals and the diameter of the resulting channels. Any suitable duration can be used, provided it is sufficient to induce channel formation within the scaffold. In some embodiments, the additional cooling step is performed for 5 minutes to 96 hours. In some embodiments, the additional cooling step is performed for 10 minutes to 60 hours. In some embodiments, the additional cooling step is performed for 1 hour to 96 hours. In some embodiments, the additional cooling step is performed for 1 hour to 60 hours. In some embodiments, the additional cooling step is performed for 12 hours to 50 hours. In some embodiments, the additional cooling step is performed for 24 hours to 48 hours. In some embodiments, the additional cooling step is performed for 36 hours to 50 hours. In some embodiments, the additional cooling step is performed for 48 hours to 60 hours.
[0064] As mentioned above, in certain embodiments, the scaffold further comprises a channel. The diameter of the channel may vary depending on the fiber-forming molecule, the solvent, the duration of the additional cooling step, and the diameter of the solvent crystals. In one embodiment, the channel has a diameter of 20 nm to 2 cm, 20 nm to 1 cm, 20 nm to 500 μm, 20 nm to 400 μm, 20 nm to 300 μm, 20 nm to 200 μm, or 20 nm to 100 μm. In one embodiment, the channel has a diameter of 10 μm to 4 mm, 10 μm to 3 mm, 10 μm to 2 mm, or 10 μm to 1 mm. In some embodiments, the channel has a diameter of 20 nm to 4 mm. In some embodiments, the channel has a diameter of 10 μm to 2 mm. In some embodiments, the channel has a diameter of 50 μm to 1 mm. In some embodiments, the channel has a diameter of 100 μm to 1000 μm. In some embodiments, the channels have a diameter of 100 μm to 800 μm. In some embodiments, the channels have a diameter of 100 μm to 600 μm. In some embodiments, the channels have a diameter of 100 μm to 400 μm. In some embodiments, the channels have a diameter of 20 nm to 2 mm. In some embodiments, the channels have a diameter of 20 nm to 1 mm. In some embodiments, the channels have a diameter of 400 μm to 1000 μm. In some embodiments, the channels have a diameter of 400 μm to 800 μm.
[0065] Advantageously, the inventors have found that in embodiments where the scaffold comprises aligned fibers and channels within the scaffold, the scaffold of the present invention had significantly higher cell viability than a scaffold comprising aligned fibers but no channels. In some embodiments, the scaffold comprising aligned fibers and channels showed improved cell capture and proliferation. In some embodiments, the aligned fibers and co-aligned channels can induce cell migration and tissue infiltration, thus promoting the regeneration or re-establishment of function of damaged tissue. The scaffold of the present invention may be useful in wound repair (radial tissue growth can aid wound closure) and may aid in the repair of cracked bone.
[0066] (Fibril-forming molecules) The scaffolds of the present invention and methods for their preparation can be prepared using any suitable fiber-forming molecule, in some embodiments, the fiber-forming molecule is selected from the group consisting of natural polymers, synthetic polymers, and combinations thereof.
[0067] Natural polymers may include polysaccharides, polypeptides, glycoproteins and their derivatives and copolymers. Polysaccharides may include agar, alginate, chitosan, hyaluronan, cellulosic polymers (e.g., cellulose and its derivatives, and cellulose production by-products such as lignin) and starch polymers. Polypeptides may include various proteins such as silk fibroin, lysozyme, collagen, keratin, casein, gelatin and their derivatives. Derivatives of natural polymers such as polysaccharides and polypeptides may include various salts, esters, ethers and graft copolymers. Exemplary salts may be selected from sodium, zinc, iron and calcium salts.
[0068] In certain embodiments, the natural polymer is selected from the group consisting of at least one of silk fibroin, alginate, bovine serum albumin, collagen, chitosan, gelatin, sericin, hyaluronic acid, starch, and derivatives thereof. In certain embodiments, the natural polymer is selected from the group consisting of silk fibroin, alginate, gelatin, silk fibroin / alginate, silk fibroin / bovine serum albumin, silk fibroin / collagen, silk fibroin / chitosan, silk fibroin / gelatin, and derivatives thereof.
[0069] Synthetic polymers may include vinyl polymers such as, but not limited to, polyethylene, polypropylene, poly(vinyl chloride), polystyrene, polytetrafluoroethylene, poly(α-methylstyrene), poly(acrylic acid), poly(methacrylic acid), poly(isobutylene), poly(acrylonitrile), poly(methyl acrylate), poly(methyl methacrylate), poly(acrylamide), poly(methacrylamide), poly(1-pentene), poly(1,3-butadiene), poly(vinyl acetate), poly(2-vinylpyridine), poly(vinyl alcohol), poly(vinylpyrrolidone), poly(styrene), poly(styrenesulfonate) poly(vinylidenehexafluoropropylene), 1,4-polyisoprene, and 3,4-polychloroprene. Suitable synthetic polymers may also include non-vinyl polymers, such as, but not limited to, poly(ethylene oxide), polyformaldehyde, polyacetaldehyde, poly(3-propionate), poly(10-decanoate), poly(ethylene terephthalate), polycaprolactam, poly(11-undecanoamide), poly(hexamethylene sebacamide), poly(m-phenylene terephthalate), poly(tetramethylene-m-benzenesulfonamide). Copolymers of any of the foregoing may also be used.
[0070] The synthetic polymers used in the process of the present invention may be classified into any of the following polymer classes: polyolefins, polyethers (including all epoxy resins, polyacetals, poly(orthoesters), polyetheretherketones, polyetherimides, poly(alkylene oxides) and poly(arylene oxides)), polyamides (including polyureas), polyamideimides, polyacrylates, polybenzimidazoles, polyesters (e.g., polylactic acid (PLA), polyglycolic acid (PGA), polylactic-glycolic acid copolymers (PLGA)), polycarbonates, polyurethanes, polyimides, polyamines, polyhydrazides, phenolics, polysilanes, polysiloxanes, polycarbodiimides, polyimines (e.g., polyethyleneimine), azopolymers, polysulfides, polysulfones, polyethersulfones, oligomeric silsesquioxane polymers, polydimethylsiloxane polymers and copolymers thereof.
[0071] In some embodiments, functionalized synthetic polymers may be used. In such embodiments, the synthetic polymers may be modified with one or more functional groups. Examples of functional groups include boronic acid, alkyne, or azide functional groups. Such functional groups are generally covalently attached to the polymer. The functional groups may allow the polymer to undergo further reactions or to impart additional properties to the fiber.
[0072] In some embodiments, the fiber-forming liquid comprises a water-soluble or water-dispersible polymer or a derivative thereof. In some embodiments, the fiber-forming liquid is a polymer solution comprising a water-soluble or water-dispersible polymer or a derivative thereof dissolved in an aqueous solvent. Exemplary water-soluble or water-dispersible polymers that may be present in the fiber-forming liquid, such as a polymer solution, may be selected from the group consisting of polypeptides, alginates, chitosan, starch, collagen, polyurethanes, polyacrylic acids, polyacrylates, polyacrylamides (including poly(N-alkylacrylamides), e.g., poly(N-isopropylacrylamide)), poly(vinyl alcohol), polyallylamine, polyethyleneimine, poly(vinylpyrrolidone), poly(lactic acid), poly(ethylene-co-acrylic acid), and copolymers thereof, and combinations thereof. Derivatives of water-soluble or water-dispersible polymers may include various salts thereof.
[0073] In some embodiments, the fiber-forming liquid comprises an organic solvent-soluble polymer. In some embodiments, the fiber-forming liquid is a polymer solution comprising an organic solvent-soluble polymer dissolved in an organic solvent. Exemplary organic solvent-soluble polymers that may be present in a fiber-forming liquid, such as a polymer solution, include poly(styrene) and polyesters, such as poly(lactic acid), poly(glycolic acid), poly(caprolactone), and copolymers thereof, such as polylactic-co-glycolic acid.
[0074] In some embodiments, the fiber-forming liquid comprises a hybrid polymer. The hybrid polymer may be an inorganic / organic hybrid polymer. Exemplary hybrid polymers include polysiloxanes, such as poly(dimethylsiloxane) (PDMS).
[0075] In some embodiments, the fiber-forming liquid comprises at least one polymer selected from the group consisting of polypeptides, alginates, chitosan, starch, collagen, silk fibroin, polyurethanes, polyacrylic acids, polyacrylates, polyacrylamides, polyesters, polyolefins, boronic acid functionalized polymers, polyvinyl alcohols, polyallylamine, polyethyleneimines, poly(vinylpyrrolidone), poly(lactic acid), polyethersulfones, and inorganic polymers.
[0076] In some embodiments, the fiber-forming solution comprises a mixture of two or more polymers, for example, a mixture of a thermoresponsive synthetic polymer (e.g., poly(N-isopropylacrylamide)) and a natural polymer (e.g., a polypeptide). The use of a polymer blend can be advantageous because it provides a means to create polymer fibers with different physical properties (e.g., thermoresponsive and biocompatible or biodegradable properties). Thus, the process of the present invention can be used to form aligned fibers with tunable or tailored physical properties by selecting an appropriate blend or mixture of polymers.
[0077] The polymers used in the process of the present invention may include homopolymers, random copolymers, block copolymers, alternating copolymers, random tripolymers, block tripolymers, alternating tripolymers, derivatives thereof (e.g., salts, graft copolymers, esters or ethers thereof), etc. of any of the aforementioned polymers. The polymers may be capable of crosslinking in the presence of a multifunctional crosslinking agent.
[0078] The fiber-forming molecules used in the process can be of any suitable molecular weight, and molecular weight is not considered a limiting factor, provided that the method of the invention is capable of aligning fibers within the scaffold. The number average molecular weight can range from a few hundred Daltons (e.g., 250 Da) to more than a few thousand Daltons (e.g., more than 10,000 Da), although any molecular weight can be used without departing from the invention. In some embodiments, the number average molecular weight is from about 50 to about 1×107 In some embodiments, the number average molecular weight may range from about 1×10 4 From about 1×10 7 The range may be:
[0079] (Additives) The scaffold of the present invention and its preparation method can include additives. Any suitable additives can be added to impart functionality to the scaffold, such as having a desired biological activity, improving the solubility of fiber-forming molecules, or promoting the formation of fibers and / or channels within the scaffold. In some embodiments, the additive is selected from the group consisting of drugs, growth factors, polymers, surfactants, chemicals, particles, porogens, and combinations thereof.
[0080] Additives can be added to the scaffold of the present invention by any method known in the art. In one embodiment, additives can be added to the scaffold by dissolving or dispersing the additive in a solution containing fiber-forming molecules. Scaffolds formed using the methods of the present invention encapsulate the additive during a cooling step. In another embodiment, additives can be added to the scaffold during an additional cooling step. Additives can be added by exposing the scaffold to a solution containing the additive, followed by an additional cooling step to induce solvent crystallization and channels within the scaffold. In another embodiment, additives in solution are contacted with the scaffold such that a certain amount of additive in the solution is adsorbed, absorbed or dispersed into the pores of the scaffold. Adsorption or absorption of additives in solution can be added to the scaffold by any suitable technique known in the art, such as dialysis. In certain embodiments, additives can be added to the scaffold by chemical reaction, such as catalysis on the scaffold to introduce the desired additive.
[0081] The term "drug" as used herein refers to a molecule, group of molecules, complex, substance or derivatives thereof that is administered to an organism for diagnostic, therapeutic, preventive medical or veterinary purposes.
[0082] Drugs can act to control infection or inflammation, enhance cell proliferation and tissue regeneration, control tumor growth, act as analgesics, promote anti-cell adhesion, and enhance bone growth, among other functions. Other suitable drugs may include antiviral agents, hormones, antibodies, or therapeutic proteins. Other drugs include prodrugs, which are agents that are not biologically active when administered, but are converted into drugs by metabolism or some other mechanism after administration to a subject.
[0083] Drugs may also specifically include nucleic acids and nucleic acid-containing compounds that produce bioactive effects, such as deoxyribonucleic acid (DNA), ribonucleic acid (RNA), or mixtures or combinations thereof, including, for example, DNA nanoplexes. Drugs include the categories and specific examples disclosed herein. It is not intended that the categories be limited by the specific examples. Those skilled in the art will recognize many other compounds that fall within the categories and are useful according to the present invention.
[0084] Examples of drugs include radiosensitizers, steroids, xanthines, beta-2-agonist bronchodilators, anti-inflammatory agents, analgesics, calcium antagonists, angiotensin converting enzyme inhibitors, beta blockers, centrally acting alpha agonists, alpha-1-antagonists, anticholinergic / antispasmodics, vasopressin analogs, antiarrhythmic agents, antiparkinsonian agents, antianginal / antihypertensive agents, anticoagulants, antiplatelet agents, sedatives, antianxiety agents, peptide agents, biopolymer agents, antitumor agents, laxatives, antidiarrheals, antimicrobial agents, antifungal agents, vaccines, proteins, or nucleic acids. In other embodiments, the drug is selected from the group consisting of coumarins, albumins, steroids such as betamethasone, dexamethasone, methylprednisolone, prednisolone, prednisone, triamcinolone, budesonide, hydrocortisone and pharma- ceutically acceptable hydrocortisone derivatives; xanthines such as theophylline and doxofylline; beta-2-agonist bronchodilators such as salbutamol, phenterol, clenbuterol, bambuterol, salmeterol, fenoterol; anti-inflammatory agents such as anti-asthmatic anti-inflammatory agents, anti-arthritic anti-inflammatory agents and non-steroidal anti-inflammatory agents (examples of which include, but are not limited to, sulfides, mesalamine, budesonide, salazopyrin, diclofenac, pharma-ceutically acceptable diclofenac salts, nimesulide, naproxen, acetominophen, ibuprofen, ketoprofen, and piroxicam); analgesics such as salicylates; calcium channel blockers such as nifedipine, amlodipine and nicardipine; angiotensin-converting enzyme inhibitors such as captopril, benazepril hydrochloride, fosinopril sodium, trandolapril, ramipril, lisinopril, enalapril, quinapril hydrochloride and moexipril hydrochloride; beta-blockers (i.e. beta-adrenergic blockers) such as sotalol hydrochloride, timolol maleate, esmolol hydrochloride, carteolol, propanolol hydrochloride, betaxolol hydrochloride, penbutolol sulfate, metoprolol tartrate, metoprolol succinate, acebutolol hydrochloride, atenolol, pindolol and bisoprolol fumarate; centrally acting alpha-2-agonists such as clonidine;Alpha-1-antagonists, such as doxazosin and prazosin; anticholinergic / antispasmodics, such as dicyclomine hydrochloride, scopolamine hydrobromide, glycopyrrolate, clidinium bromide, flavoxate and oxybutynin; vasopressin analogues, such as vasopressin and desmopressin; antiarrhythmics, such as quinidine, lidocaine, tocainide hydrochloride, mexiletine hydrochloride, digoxin, verapamil hydrochloride, propafenone hydrochloride, flecainide acetate, procainamide hydrochloride, moricizine. hydrochlorides and disopyramide phosphates;antiparkinsonian drugs such as dopamine, L-dopa / carbidopa, selegiline, dihydroergocryptine, pergolide, lisuride, apomorphine and bromocriptine;antianginal and antihypertensive drugs such as isosorbide mononitrate, isosorbide dinitrate, propranolol, atenolol and verapamil;anticoagulants and antiplatelet agents such as coumadin, warfarin, acetylsalicylic acid and ticlopidine;sedatives such as benzodiazapines and barbiturates;antianxiety drugs such as benzodiazapines and barbiturates. agents, such as lorazepam, bromazepam, and diazepam; peptide and biopolymer agents, such as calcitonin, leuprolide and other LHRH agonists, hirudin, cyclosporine, insulin, somatostatin, protirelin, interferons, desmopressin, somatotropin, thymopentin, pidotimod, erythropoietin, interleukins, melatonin, granulocyte / macrophage-CSF, and heparin; antitumor agents, such as etoposide, etoposide phosphate, cyclophosphamide, methotrexate ... oxalate, 5-fluorouracil, vincristine, doxorubicin, cisplatin, hydroxyurea, leucovorin calcium, tamoxifen, flutamide, asparaginase, altretamine, mitotane and procarbazine hydrochloride; laxatives such as senna concentrate, casanthranol, bisacodyl and sodium picosulfate; antidiarrheals such as difenoxin hydrochloride, loperamide hydrochloride, furazolidone, diphenoxylate hydrochloride and microorganisms; vaccines such as bacterial and viral vaccines;Antimicrobial agents, such as penicillins, cephalosporins and macrolides, antifungal agents, such as imidazole and triazole derivatives; and nucleic acids, such as DNA sequences encoding biological proteins, and antisense oligonucleotides.
[0085] Growth factors as additives suitable for the present invention can stimulate cell growth, proliferation, healing or differentiation. Growth factors can be proteins or steroid hormones. For example, growth factors can be bone morphogenetic proteins that stimulate bone cell differentiation. In addition, fibroblast growth factors and vascular endothelial growth factors can stimulate blood vessel differentiation (angiogenesis).
[0086] Growth factors include adrenomedullin, angiopoietin, autocrine motility stimulating factor, bone morphogenetic proteins, ciliary neurotrophic factor family (e.g., ciliary neurotrophic factor, leukemia inhibitory factor, interleukin-6), colony-stimulating factors (e.g., macrophage colony-stimulating factor, granulocyte colony-stimulating factor, and granulocyte-macrophage colony-stimulating factor), epidermal growth factor, ephrins (ephrin A1, ephrin A2, ephrin A3, ephrin A4, ephrin A5, ephrin B1, ephrin B2, and ephrin B3), erythropoietin, fibroblast growth factors (fibroblast growth factor 1, fibroblast growth factor 2, and fibroblast growth factor 3), and fibroblast growth factor 4. , fibroblast growth factor 3, fibroblast growth factor 4, fibroblast growth factor 5, fibroblast growth factor 6, fibroblast growth factor 7, fibroblast growth factor 8, fibroblast growth factor 9, fibroblast growth factor 10, fibroblast growth factor 11, fibroblast growth factor 12, fibroblast growth factor 13, fibroblast growth factor 14, fibroblast growth factor 15, fibroblast growth factor 16, fibroblast growth factor 17, fibroblast growth factor 18, fibroblast growth factor 19, fibroblast growth factor 20, fibroblast growth factor 21, fibroblast growth factor 22 and fibroblast growth factor 23), fetal bovine somatotropin (FSO4),somatotrophin), the GDNF family of ligands (such as glial cell line-derived neurotrophic factor (GDNF), neurturin, persephin, and artemin), growth differentiation factor-9, hepatocyte growth factor, hepatoma cell-derived growth factor, insulin, insulin-like growth factors (such as insulin-like growth factor-1 and insulin-like growth factor-2), interleukins (such as IL-1, IL-2, IL-3, IL-4, IL-5, IL-6, and IL-7), keratinocyte growth factor, migration stimulating factor, macrophage stimulating protein The inhibitor may be selected from the group consisting of: lipids, myostatin, neuregulins (such as neuregulin 1, neuregulin 2, neuregulin 3 and neuregulin 4), neurotrophins (such as brain-derived neurotrophic factor, nerve growth factor, neurotrophin-3, neurotrophin-4), placental growth factor, platelet-derived growth factor, renalase, T cell growth factor, thrombopoietin, transforming growth factors (such as transforming growth factor alpha and transforming growth factor beta), tumor necrosis factor alpha, vascular endothelial growth factor and combinations thereof.
[0087] The scaffold may also contain adjuvants such as preservatives, wetting agents, emulsifying agents and dispersing agents. Prevention of the action of microorganisms may be ensured by including various antibacterial and antifungal agents, for example, paraben, chlorobutanol, phenol sorbic acid, etc. It may also be desirable to include isotonic agents, such as sugars, sodium chloride, etc.
[0088] A person skilled in the relevant art will understand that polymers suitable as additives in the present invention may be those already mentioned above in connection with fiber-forming molecules.
[0089] Surfactants as additives suitable for the present invention can increase the solubility of fiber-forming molecules. Without wishing to be bound by any theory, the inventors believe that surfactants can reduce the self-aggregation of fiber-forming molecules and increase the solubility of the solution containing the fiber-forming molecules. In one embodiment, the surfactant is anionic, cationic, zwitterionic or nonionic. In one embodiment, the surfactant comprises a functional group selected from the group consisting of sulfate, sulfonate, phosphate, carboxylate, amine, ammonium, alcohol, ether and combinations thereof. In one embodiment, the surfactant is selected from the group consisting of sodium stearate, sodium dodecyl sulfate, cetrimonium bromide, 4-(5-dodecyl)benzenesulfonate, 3-[(3-cholamidopropyl)dimethylammonio]-1-propanesulfonate, phosphatidylserine, phosphatidylethanolamine, phosphatidylcholine, octaethylene glycol monododecyl ether, pentaethylene glycol monododecyl ether, decyl glucoside, lauryl glucoside, octyl glucoside, Triton X-100, nonoxynol-9, glyceryl laurate, polysorbates, dodecyldimethylamine oxide, polysorbates (such as polysorbate 20 and polysorbate 80, commercially available as Tween 20 and Tween 80), cocamide monoethanolamine, cocamide diethanolamine, poloxamer, polyethoxylated tallow amine, and combinations thereof.
[0090] Scaffolds with Aligned Fibers and a Central Channel In certain embodiments, the scaffold of the present invention may further comprise a central channel. The central channel may be directed along the axis of the scaffold, such as the longitudinal axis of the scaffold. The central channel may be formed using any suitable technique known in the art. In certain embodiments, the central channel may be formed by mechanical processing, such as using a blade or laser to cut the scaffold to form the channel. In other embodiments, the central channel is formed by controlling the cooling of the solution containing the fiber-forming molecules once the scaffold is formed, such that the cooling process ends before the scaffold is fully formed and the central channel is generated. Alternatively, the central channel may be formed upon cooling the fiber-forming solution using a cylindrical tube as a container with an inner tube or cylinder that defines the shape of the central channel.
[0091] The central channel can be of any suitable dimension. In certain embodiments, the central channel has a diameter greater than 0.1 mm, 0.4 mm, 0.8 mm, 1 cm, or 2 cm. In certain embodiments, the central channel has a diameter between 0.1 mm and 2 cm. In certain embodiments, the central channel has a diameter between 0.1 mm and 1 cm. In certain embodiments, the central channel has a diameter between 0.1 and 4 mm. In certain embodiments, the central channel has a diameter between 0.2 and 4 mm. In certain embodiments, the central channel has a diameter between 0.1 and 2 mm. In certain embodiments, the central channel has a diameter between 0.4 and 2 mm. In certain embodiments, the central channel has a diameter between 0.4 and 1 mm. In certain embodiments, the central channel has a diameter between 0.4 and 0.8 mm.
[0092] (Cell culture, cell proliferation and tissue repair) The scaffold of the present invention can be suitable for promoting cell proliferation, cell culture and tissue formation in bulk 3D scaffold.Therefore, the cells attached to the scaffold of the present invention have any desired cell viability and are determined based on the desired application.As will be understood by those skilled in the art, cells can be cultured on the scaffold of the present invention using any suitable technique known in the art.Typically, cells can be cultured on the scaffold after the formation of the scaffold.
[0093] It is understood that any suitable cells can be used for cell culture on the scaffold of the present invention. The type of cells used is determined based on the application of the scaffold. In certain embodiments, the present invention can provide a method for promoting cell proliferation, comprising capturing and culturing cells within the scaffold of the present invention. In certain embodiments, the cells are selected from neural cells, skin cells, fibroblasts, vascular cells, endothelial cells, bone cells, muscle cells, cardiac cells, corneal cells, tympanic membrane cells, cancer cells, and combinations thereof. In certain embodiments, the cells are selected from neural cells, fibroblasts, endothelial cells, stem cells, progenitor cells, and combinations thereof.
[0094] In some embodiments, the method of promoting cell proliferation comprises promoting nerve repair or regeneration, where the cell is a nerve cell. In some embodiments, the method of promoting cell proliferation comprises promoting blood vessel repair or formation, where the cell is an endothelial cell.
[0095] In some embodiments, the present invention may provide a use of the scaffold of the present invention in the preparation of a biomedical implant for promoting cell growth, comprising capturing and culturing cells. In some embodiments, the use comprises promoting nerve repair or regeneration, wherein the cells are neuronal cells. In some embodiments, the use comprises promoting blood vessel repair or formation, wherein the cells are endothelial cells.
[0096] As will be apparent to one of ordinary skill in the relevant art, the scaffold can be used in any suitable application for cell culture, tissue regeneration or tissue repair. In some embodiments, the scaffold can be used as a biomedical implant. In some embodiments, the scaffold can be used as a vascular graft. In certain embodiments, the scaffold can be used for wound healing, bone injury repair, treatment of injured tissue, drug delivery or in vitro cell culture. The scaffold can be used as a substrate for in vitro cell culture by providing a coating or layer of the scaffold on cell culture dishes, plates and flasks. Advantageously, in embodiments where the fibers are radially aligned, the scaffold can be used in tissue or wound repair, as the radial fibers can promote wound closure.
[0097] In one embodiment, the present invention provides a method of treating a mammal having suffered tissue damage and in need of tissue repair and / or regeneration, the method comprising applying a scaffold of the present invention to the site of the damage.
[0098] In one embodiment, the present invention provides the use of a scaffold of the present invention in the treatment of tissue damage and in the preparation of a biomedical implant for the repair and / or regeneration of tissue.
[0099] In one embodiment, the present invention provides the use of a scaffold for treating a mammalian subject that has suffered tissue damage and is in need of tissue repair and / or regeneration, comprising applying a scaffold of the present invention to the site of damage.
[0100] When the scaffold or biomedical implant is used for tissue engineering or tissue repair and / or regeneration applications, the method can be performed, for example, by implanting the scaffold (i.e., a porous biocompatible scaffold that does not cause an acute reaction when implanted in a patient) or biomedical implant into a mammal and then removing the scaffold or biomedical implant from the mammal (such as a human). The scaffold or biomedical implant is implanted in direct contact (i.e., in physical contact with at least a portion of its outer surface) or adjacent (i.e., physically separated) from the mature or immature target tissue for a sufficient time to allow cells of the target tissue to bind to the scaffold or biomedical implant. In some embodiments, the scaffold or biomedical implant can be pre-seeded with cells of the target tissue. The tissue graft comprises the removed scaffold and associated cells of the target tissue.
[0101] A "target tissue" is any type of tissue for which a graft is generated to replace it. For example, if a patient tears or otherwise damages a ligament and the ligament is targeted for replacement with a graft created by the methods described herein, the target tissue is a ligament. If a patient damages cartilage, the target tissue is cartilage, if a patient damages a tendon, the target tissue is tendon, and so on. A target tissue is "mature" if it contains cells and other components naturally found in fully differentiated tissues (e.g., a recognizable ligament in an adult mammal is a mature target tissue). A target tissue is "immature" if it contains cells that have not yet differentiated into mature cells, but will differentiate into mature cells (e.g., an immature target tissue can contain mesenchymal stem cells, bone marrow stromal cells, and precursor or progenitor cells). A target tissue is also "immature" if it contains cells that differentiate immature cells into cells of the mature target tissue or if it contains cells that maintain mature cells (these events can occur, for example, when cells secrete growth factors or cytokines that result in cell differentiation or maintain mature cells). Thus, the scaffold or biomedical implant of the present invention can be realized by implanting the scaffold or biomedical implant comprising the scaffold of the present invention in direct contact with or adjacent to the target tissue or tissue containing cells that can generate the target tissue (e.g., by differentiation, a process described herein, or by the action of growth factors or cytokines).
[0102] In some embodiments, the mammal having the tissue defect and the mammal from which the tissue graft is obtained can be the same mammal or the same type of mammal (e.g., one human patient can have a tissue defect that is to be treated with a graft generated using another human), or the mammal having the tissue defect and the mammal from which the tissue graft is obtained can be different types of mammal (e.g., a human patient can have a tissue defect that is to be treated with a graft generated using another primate, cow, horse, sheep, pig, or goat).
[0103] Once obtained, the scaffold or biomedical implant can be implanted into a mammal at the site of the tissue defect by any surgical technique. For example, the scaffold or biomedical implant can be sutured, pinned, fastened, or stapled to the mammal at the site of the tissue defect. In one embodiment, the scaffold or biomedical implant is implanted by attaching a first portion of the scaffold or biomedical implant to a first support structure at the site of the tissue defect and attaching a second portion of the scaffold or biomedical implant to a second support structure at the site of the tissue defect, such that the scaffold or biomedical implant connects the first support structure to the second support structure.
[0104] If the first support structure is the tibia, the second support structure can be the femur. If the first support structure is a first articular surface of a joint (e.g., a shoulder, wrist, elbow, hip, knee or ankle joint), the second support structure can be a second articular surface of the same joint (i.e., a shoulder, wrist, elbow, hip, knee or ankle joint, respectively).
[0105] The term "adjacent" as used herein means that the scaffold or biomedical implant is separated from the target type tissue, or tissue containing cells capable of generating the target type tissue, or both, if present, by a distance of up to 10 mm, preferably less than 5 mm.
[0106] The viability of cells attached to the scaffold or biomedical implant can be measured using any suitable technique known in the art. Cell viability can be measured using colorimetric assays, such as MTT (3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide) assay, XTT (2,3-bis-(2-methoxy-4-nitro-5-sulfophenyl)-2H-tetrazolium-5-carboxanilide) assay, MTS (3-(4,5-dimethylthiazol-2-yl)-5-(3-carboxymethoxyphenyl)-2-(4-sulfophenyl)-2H-tetrazolium) assay, WST (water-soluble tetrazolium salt) assay, etc. Alternatively, cell viability can be evaluated using microscopic techniques involving cell staining to distinguish between live and dead cells.
[0107] (composite material) The present invention also relates to modified materials, such as fabrics, bandages or other existing products, having various types and compositions of the fibers described herein to produce composites, such as biomimetic composites. In one embodiment, the present invention provides a composite material comprising a matrix of substantially aligned fibers and at least one substrate.
[0108] In some embodiments, the composite material is porous. In some embodiments, the composite material is non-porous. It is understood that the composite material is suitable for promoting cell growth and / or tissue formation.
[0109] The composite materials of the present invention can be used for disease treatment, wound healing, tissue regeneration, drug delivery, etc. For composite materials that include textiles as substrates, properties including feel, comfort, breathability, mechanical properties, antimicrobial (e.g., antiviral, antibacterial, and antialgal) properties, hydrophobicity, and hydrophilicity can be tailored. In some embodiments, the composite materials can be used as bandages or dressings for wound healing, tissue regeneration, and treatment of diseases such as diabetes.
[0110] The composite materials of the present invention can include any suitable amount of fibers, and the functional aspects of the composite materials, including cell adhesion, proliferation, growth, differentiation, antimicrobial function, and tissue regeneration, can be tailored depending on the amount of aligned fibers and fiber-forming solution used.
[0111] One of skill in the art will appreciate that the composite materials of the present invention can include additives such as drugs or growth factors that may be beneficial for cell adhesion, proliferation, growth, differentiation, tissue regeneration, or antimicrobial properties. In some embodiments, additives can be added to a solution of fiber-forming molecules to provide aligned fibers with the additives added, adsorbed, or absorbed into the composite material.
[0112] Typically, a substrate is immersed in a solution of fiber-forming molecules which is then cooled using the present invention to provide a composite material having aligned fibers.
[0113] (base material) The substrate can be any suitable material suitable as a template for incorporating the aligned fibers of the present invention. Examples of substrates include bandages, dressings, and textiles. In some embodiments, the substrate can be a scaffold prepared by the method of the present invention. The substrate can be any suitable material, porous or non-porous, that can incorporate aligned fibers into the composite material of the present invention. In certain embodiments, the substrate can be porous or non-porous. In embodiments where the substrate is non-porous, aligned fibers can be formed on the surface of the substrate. In embodiments where the substrate is porous, aligned fibers can be formed within the pores and / or on the surface of the substrate. When aligned fibers are formed on the surface of the substrate, the aligned fibers can form a scaffold if there are sufficient fiber-forming molecules.
[0114] The present invention can provide aligned fibers more uniformly and robustly on or within a substrate than techniques known to those skilled in the art, including deposition, dispersion and coating techniques. Advantageously, the present invention is easy, efficient and cost-effective for large-scale modification of a variety of substrates to provide the resulting composite materials.
[0115] In some embodiments, the substrate is selected from the group consisting of natural polymers, synthetic polymers, and combinations thereof.
[0116] Natural polymers may include polysaccharides, polypeptides, glycoproteins and their derivatives and copolymers. Polysaccharides may include agar, alginate, chitosan, hyaluronan, cellulosic polymers (e.g., cellulose and its derivatives, and cellulose production by-products such as lignin) and starch polymers. Polypeptides may include various proteins such as silk fibroin, silk sericin, lysozyme, collagen, keratin, casein, gelatin and their derivatives. Derivatives of natural polymers such as polysaccharides and polypeptides may include various salts, esters, ethers and graft copolymers. Exemplary salts may be selected from sodium, zinc, iron and calcium salts.
[0117] In certain embodiments, the natural polymer is selected from the group consisting of at least one of silk fibroin, alginate, bovine serum albumin, collagen, chitosan, gelatin, sericin, hyaluronic acid, starch, and derivatives thereof. In certain embodiments, the natural polymer is selected from the group consisting of silk fibroin, alginate, gelatin, silk fibroin / alginate, silk fibroin / bovine serum albumin, silk fibroin / collagen, silk fibroin / chitosan, silk fibroin / gelatin, and derivatives thereof.
[0118] Synthetic polymers may include vinyl polymers such as, but not limited to, polyethylene, polypropylene, poly(vinyl chloride), polystyrene, polytetrafluoroethylene, poly(α-methylstyrene), poly(acrylic acid), poly(methacrylic acid), poly(isobutylene), poly(acrylonitrile), poly(methyl acrylate), poly(methyl methacrylate), poly(acrylamide), poly(methacrylamide), poly(1-pentene), poly(1,3-butadiene), poly(vinyl acetate), poly(2-vinylpyridine), poly(vinyl alcohol), poly(vinylpyrrolidone), poly(styrene), poly(styrenesulfonate) poly(vinylidenehexafluoropropylene), 1,4-polyisoprene, and 3,4-polychloroprene. Suitable synthetic polymers may also include non-vinyl polymers, such as, but not limited to, poly(ethylene oxide), polyformaldehyde, polyacetaldehyde, poly(3-propionate), poly(10-decanoate), poly(ethylene terephthalate), polycaprolactam, poly(11-undecanoamide), poly(hexamethylene sebacamide), poly(m-phenylene terephthalate), poly(tetramethylene-m-benzenesulfonamide). Copolymers of any of the foregoing may also be used.
[0119] The synthetic polymers used in the process of the present invention may be classified into any of the following polymer classes: polyolefins, polyethers (including all epoxy resins, polyacetals, poly(orthoesters), polyetheretherketones, polyetherimides, poly(alkylene oxides) and poly(arylene oxides)), polyamides (including polyureas), polyamideimides, polyacrylates, polybenzimidazoles, polyesters (e.g., polylactic acid (PLA), polyglycolic acid (PGA), polylactic-glycolic acid copolymers (PLGA)), poly(lactide-co-ε-caprolactone) (PLCL), polycarbonates, polyurethanes, polyimides, polyamines, polyhydrazides, phenolics, polysilanes, polysiloxanes, polycarbodiimides, polyimines (e.g., polyethyleneimine), azopolymers, polysulfides, polysulfones, polyethersulfones, oligomeric silsesquioxane polymers, polydimethylsiloxane polymers and copolymers thereof.
[0120] In some embodiments, functionalized synthetic polymers may be used. In such embodiments, the synthetic polymers may be modified with one or more functional groups. Examples of functional groups include Arg-Gly-Asp (RGD) peptides, boronic acid, alkyne, amino, carboxyl or azide functional groups. Such functional groups are generally covalently attached to the polymer. The functional groups may allow the polymer to undergo further reactions or to impart additional properties to the fibers.
[0121] In some embodiments, the substrate comprises a water-soluble or water-dispersible polymer or a derivative thereof. In some embodiments, the substrate comprises a water-soluble or water-dispersible polymer or a derivative thereof. Exemplary water-soluble or water-dispersible polymers include polypeptides, alginates, chitosan, starch, collagen, polyurethane, polyacrylic acid, polyacrylates, polyacrylamides (including poly(N-alkylacrylamides), (e.g., poly(N-isopropylacrylamide)), poly(vinyl alcohol), polyallylamine, polyethyleneimine, poly(vinylpyrrolidone), poly(lactic acid), poly(ethylene-co-acrylic acid), polyesters (e.g., polylactic acid (PLA), polyglycolic acid (PGA), polylactic-co-glycolic acid (PLGA)), poly(lactide-co-ε-caprolactone) (PLCL), polycarbonates, polyurethanes, polypropylenes) and copolymers thereof and combinations thereof. Derivatives of water-soluble or water-dispersible polymers may include various salts thereof.
[0122] In some embodiments, the substrate comprises an organic solvent soluble polymer selected from the group consisting of poly(styrene) and polyesters, such as poly(lactic acid), poly(glycolic acid), poly(caprolactone) and copolymers thereof, such as polylactic-co-glycolic acid.
[0123] In some embodiments, the substrate comprises a hybrid polymer. The hybrid polymer may be an inorganic / organic hybrid polymer. Exemplary hybrid polymers include polysiloxanes, such as poly(dimethylsiloxane) (PDMS).
[0124] In some embodiments, the substrate comprises at least one polymer selected from the group consisting of polypeptides, alginates, gelatin, chitosan, starch, collagen, silk fibroin, polyurethane, polyacrylic acid, polyacrylates, polypropylene, polyacrylamide, polyesters, polyolefins, boronic acid functionalized polymers, polyvinyl alcohol, polyallylamine, polyethyleneimine, poly(vinylpyrrolidone), poly(lactic acid), polyethersulfone, and inorganic polymers.
[0125] In some embodiments, the substrate comprises a mixture of two or more polymers, for example, a mixture of a thermoresponsive synthetic polymer (eg, poly(N-isopropylacrylamide)) and a natural polymer (eg, a polypeptide).
[0126] Examples of materials and methods for use with the methods of the present invention are provided below. In providing these examples, it is understood that the specific nature of the following descriptions does not limit the generality of the above descriptions.
[0127] (Example) The invention will now be described with reference to the following examples.
[0128] (Preparation of silk fibroin (SF) solution) The silk cocoons were boiled four times (20 min / h) in 0.5% (w / v) Na2CO3 aqueous solution to remove sericin proteins. The degummed silk fibers were thoroughly rinsed with ultrapure water to remove residual sericin. After drying, they were dissolved in a mixture of CaCl2, H2O and CH3CH2OH (molar ratio 1:8:2) at 65 °C to obtain a clear solution. The resulting solution was then dialyzed against ultrapure water (18.2 mΩ·cm) using cellulose dialysis tubing (molecular weight cut-off: 14 kDa; Sigma Aldrich, Australia) for 4 days at ambient temperature. Impurities were filtered and removed by centrifugation at 5000 rpm for 20 min. Finally, the regenerated SF sponge was obtained by freeze-drying the centrifuged solution using a freeze dryer (FreeZone 2.5 L benchtop freeze dryer; Labconco, Kansas City, MO, USA). For subsequent use, a SF solution (2%) was obtained by dissolving 2 g of regenerated SF sponge in 100 mL of ultrapure water.
[0129] Preparation of 3D SF scaffolds (a) Scaffold with aligned nanofibers (AFb) The SF solution in the glass tube was directly immersed in liquid nitrogen. The frozen samples were freeze-dried using a freeze dryer to generate the targeted scaffolds. The fabrication scheme is shown in Figure 2.
[0130] (b) Water-resistant aligned nanofiber scaffold (AF). To make the scaffold insoluble in water, the above obtained scaffold (AFb) was post-treated by immersion in ethanol at ambient temperature for 12 h. After removing the ethanol and thoroughly rinsing with ultrapure water, the AF scaffold was obtained, which was re-immersed in ultrapure water for use or further processing.
[0131] (c) Scaffold with co-aligned nanofibers and macrochannels (A(F&C)). The AF scaffolds in ultrapure water were frozen for 72 hours at −20° C. After freeze-drying, the A(F&C) scaffolds were obtained.
[0132] (d) Wb and W&Fb scaffolds (Wb obtained from freezing at −20°C and W&Fb obtained from freezing at −80°C). For comparison, scaffolds were formed in freezers at -20°C and -80°C, respectively, instead of flash freezing with liquid nitrogen. For the -20°C Wb scaffold, the SF solution in a glass tube was frozen at -20°C for 53 hours. For the -80°C W&Fb scaffold, the SF solution in a glass tube was frozen at -80°C for 53 hours. After removal of ice crystals by freeze-drying, the Wb and W&Fb scaffolds are obtained, respectively.
[0133] (e) W and W&F scaffolding The above Wb and W&Fb scaffolds were further processed using the same procedure to obtain A(F&C) scaffolds. Namely, the scaffolds were post-treated by immersion in ethanol at ambient temperature for 12 h. After removing the ethanol and thoroughly rinsing with ultrapure water, the scaffolds in ultrapure water were frozen at -20 °C for 72 h. After freeze-drying, W and W&F scaffolds were obtained, respectively.
[0134] (3D SF / gelatin composite A(F&C) scaffold) For subsequent use, SF / gelatin (Sigma-Aldrich, Australia) solution (2%) was obtained by dissolving 2 g of regenerated SF / gelatin mixture (weight ratio 95:5) in 100 mL of ultrapure water. SF / gelatin composite A (F&C) scaffolds were then fabricated by the same protocol for generating SF A (F&C) scaffolds described above.
[0135] (3D Sodium Alginate A (F&C) Scaffold) Sodium alginate (Sigma-Aldrich, Australia) solution (0.3% w / v) was made by dissolving 0.3 g of sodium alginate in 100 mL of ultrapure water with stirring at 50 °C. Apart from the post-treatment of AFb scaffolds to form AF scaffolds using CaCl2 aqueous solution instead of ethanol, sodium alginate A (F&C) scaffolds were prepared by the same protocol to make SF A (F&C) scaffolds.
[0136] (composite material) The solution of fiber-forming molecules and the substrate (e.g., polypropylene porous microfiber material) in a container, or the substrate imbibed with the solution of fiber-forming molecules (e.g., silk fibroin solution, alginate solution, gelatin solution, or a combination thereof) were directly immersed in liquid nitrogen or slowly lowered into liquid nitrogen to create a temperature difference. Composite materials were generated by freeze-drying the frozen samples using a freeze dryer. Optionally, the resulting composite scaffolds can be post-treated by immersing them in a suitable crosslinking agent (e.g., ethanol solution) or in a crosslinking agent vapor environment (e.g., 75% ethanol vapor) to make the scaffolds insoluble in water. The resulting composite materials were obtained by drying at room temperature or rinsing thoroughly with ultrapure water and then freeze-drying. Representative micrographs are shown in Figures 4 and 5.
[0137] (Characteristics evaluation) The morphology of the materials was observed using a scanning electron microscope (SEM) (Zeiss Supra 55VP), and the fiber diameter was determined from representative SEM images by image processing software (Image-J 1.34) in attenuated total reflection (ATR) mode (4 cm -1 Resolution: 600–4000 cm (64 scans) using a Bruker VERTEX 70 instrument. -1Fourier transform infrared spectroscopy (FTIR) spectra were recorded in the wavenumber range of 100 nm to 100 nm. Compressive mechanical properties of silk scaffolds were obtained using an Instron 5967 computerized universal material testing machine (Instron Corp, USA) equipped with a 100 N loading cell. Cylindrical scaffolds with a diameter of 10 mm and a height of 4 mm were measured (six specimens were measured for each group) at a crosshead speed of 5 mm / min. Compressive stress was plotted versus strain, and the compressive modulus was calculated as the slope of the initial linear portion of the stress-strain curve. The structure of silk scaffolds was imaged using micro X-ray computed tomography (microCT) with an Xradia micro XCT200 (Carl Zeiss X-ray Microscopy, Inc., USA). An X-ray tube with a voltage of 40 kV and a peak power of 10 W was used. For one complete tomographic reconstruction, 361 isometric projections at 180 degrees (exposure time: 8 s / projection) were obtained. To obtain clear projections and final 3D visualization, a phase retrieval tomography with 3D reconstruction algorithm was introduced. The size of the reconstructed 3D image was 512 × 512 × 512 voxels with a voxel size of 4.3 μm along each side.
[0138] (Scaffold cell capture, proliferation and in vitro angiogenesis of human umbilical vein endothelial cells in 3D SF scaffolds) Culture of human umbilical vein endothelial cells (HUVECs; Life Technologies, Australia) and scaffold seeding: HUVECs were cultured in Medium 200 with low serum growth supplement (LSGS; Life Technologies, Australia). After sterilization in a 75% ethanol vapor environment, scaffolds (approximately 10 mm in diameter and 3 mm in thickness) were placed in a 24-well plate (Greiner Bio-One). HUVECs suspended in cell medium were seeded at the corresponding density (1 × 10 for in vitro cell adhesion, proliferation and angiogenesis tests, respectively). 5 / well, 1.5 x 10 5 / well and 2 × 10 5 Cells were uniformly seeded onto the scaffolds at 100 μg / well. The cell-seeded scaffolds were maintained in vitro under standard culture conditions (37 °C, 5% CO2) with medium changes every 2–3 days.
[0139] (a) Cell entrapment and proliferation on the scaffold At certain time points after seeding (2, 4, and 8 h for cell capture assays, and 2, 4, and 6 days for cell proliferation assays), the viability of cells on the scaffolds was analyzed using the MTS assay (Promega, USA) according to the manufacturer's instructions, and the absorbance was measured at 490 nm using a microplate reader (SH-1000Lab, Corona Electric Co., Ltd, Japan).
[0140] After 3 days of culture, cell morphology on the scaffolds was observed using a confocal fluorescence microscope (Leica TCS SP5 confocal microscope, Leica Microsystems, Wetzlar). The cell-scaffold complexes were rinsed with PBS and fixed with 4% paraformaldehyde (Sigma-Aldrich, Australia) for 30 min at ambient temperature. After rinsing with PBS, the complexes were permeabilized with 0.1% Triton X-100 (Sigma-Aldrich, Australia) for 10 min, followed by rinsing with PBS. The complexes were then incubated in Image-iT® FX Signal Enhancer Ready Probes™ reagent (Life Technologies, Australia) for 30 min and rinsed with PBS. The complexes were then incubated with Alexa Fluor® 568 phalloidin (1:100; Life Technologies, Australia) for 1 h. After rinsing with PBS, the complexes were incubated in DAPI (Life Technologies, Australia) for 10 min in the dark. The as-treated samples were evaluated using confocal fluorescence microscopy.
[0141] (b) In vitro vascularization within the scaffold After 21 days of culture, the cell-scaffold complexes were rinsed with PBS and fixed with 4% paraformaldehyde (Sigma-Aldrich, Australia) for 30 min at ambient temperature. After rinsing with PBS, the complexes were permeabilized with 0.1% Triton X-100 (Sigma-Aldrich, Australia) for 10 min, followed by rinsing with PBS. The complexes were then incubated in Image-iT® FX Signal Enhancer Ready Probes™ reagent (Life Technologies, Australia) for 30 min. After rinsing with PBS, the complexes were incubated with 10% normal goat serum blocking solution (Life Technologies, Australia) for 10 min to block non-specific binding, and then rinsed with PBS. The complexes were then incubated with CD31 monoclonal antibody (1:50; Life Technologies, Australia) overnight at 4°C. After rinsing with PBS, the complexes were incubated with goat anti-mouse IgG (H+L) secondary antibody, Alexa Fluor® 488 conjugate (1:200; Life Technologies, Australia) for 1 h. Scaffolds were rinsed again with PBS and incubated in DAPI (Life Technologies, Australia) for 10 min in the dark. As-treated samples were evaluated using confocal fluorescence microscopy.
[0142] Scaffold cell capture and neurite outgrowth of rat embryonic dorsal root ganglion neurons within 3D SF scaffolds. (a) Culture and scaffold seeding of rat embryonic dorsal root ganglion neurons (DRG; Lonza, USA). DRGs were cultured in Primary Neuron Basal Medium (PNBM; Lonza, USA) supplemented with PNGM™ SingleQuots™ (Lonza, USA) and 150 ng / ml nerve growth factor (NGF; Sigma-Aldrich, Australia).
[0143] After sterilization by 75% ethanol vapor, the scaffolds (diameter approx. 10 mm and thickness approx. 3 mm) were placed in a 24-well plate (Greiner Bio-One). DRG suspended in cell culture medium were added at 1.2 × 10 5 DRGs were uniformly seeded onto the scaffolds at a density of 1000 / well. DRG-seeded scaffolds were maintained in vitro under standard culture conditions (37 °C, 5% CO2) with medium changes every 3–5 days.
[0144] (b) Cell entrapment in the scaffold At certain time points after seeding (6, 12 and 24 h), the viability of DRGs entrapped in the scaffolds was analyzed using the MTS assay (Promega, USA) according to the manufacturer's instructions, and the absorbance was measured at 490 nm using a microplate reader (SH-1000Lab, Corona Electric Co., Ltd, Japan).
[0145] (c) Immunostaining for neurite outgrowth in DRG After 21 days of culture, the scaffolds were rinsed with PBS and fixed with 4% paraformaldehyde (Sigma-Aldrich, Australia) for 30 min at ambient temperature. After rinsing with PBS, the complexes were permeabilized with 0.1% Triton X-100 (Sigma-Aldrich, Australia) for 30 min and then rinsed again with PBS. The scaffolds were then incubated in 10% normal goat serum blocking solution (Life Technologies, Australia) for 10 min to block non-specific binding, followed by rinsing with PBS. The scaffolds were then incubated overnight at 4°C with rabbit-derived anti-neurofilament-200 antibody (1:50; Sigma-Aldrich, Australia). After rinsing with PBS, the scaffolds were incubated with goat anti-rabbit IgG (H+L) secondary antibody, Alexa Fluor® 488 conjugate (1:200; Life Technologies, Australia) for 1 h. Finally, the treated samples were analyzed using a confocal fluorescence microscope.
[0146] (d) Statistical methods All experiments were performed in triplicate and data were expressed as mean ± standard deviation (SD). Statistical significance was analyzed by one-way analysis of variance using statistical software from the Origin 9 software package (OriginLab, USA). Differences of p<0.05 or p<0.01 were interpreted as statistically significant.
[0147] Example 1. Silk fibroin scaffold FDA-approved silk fibroin (SF) has been widely recognized and used as a biomedical material due to its excellent biocompatibility, tunable mechanical properties, biodegradability and low inflammatory response. Using silk fibroin as a model, we demonstrated that 3D silk fibroin (SF) scaffolds with co-aligned nanofibers and macrochannels can be conveniently fabricated by a facile freeze-drying approach. The method is based on the control of ice crystallization. When a volume of water freezes, the size of the ice crystals and their orientation are controlled by the temperature gradient, the freezing rate, and the direction of the temperature gradient in that volume. The lower the temperature and the faster the freezing, i.e., the higher the thermodynamic driving force and reaction rate, the more favorable the ice nucleation and the more fine crystals there are.
[0148] Based on this principle, we employed a two-step freezing method to fabricate the desired SF structures using various fiber-forming molecules, such as silk fibroin, a mixture of silk fibroin / gelatin, and sodium alginate. A schematic diagram is shown in Figure 2. First, a tube containing an SF aqueous solution was quickly immersed in liquid nitrogen. The extremely low temperature (approximately −196 °C in liquid nitrogen) and the large temperature difference along the radial direction of the tube led to the formation of radially aligned fine ice crystals. After removing the ice crystals by freeze-drying, SF nanofibers were obtained that were radially aligned along the ice crystal growth direction.
[0149] To make the nanofibers insoluble in water, ethanol was used to fix the structure of the protein nanofibers, and then the nanofiber scaffold was placed in water and frozen again at a relatively high temperature of -20°C. This relatively high temperature led to the formation of even larger ice crystals induced by the radially aligned nanofibers to grow along the fiber direction. The formation of the crystals reduces the free space of the nanofibers, which causes the nanofibers to be pushed and squeezed around the crystals. After removing these crystals by freeze-drying, macrochannels with nanofiber walls are created in the aligned 3D nanofiber scaffold. Compared with the widely used 3D silk scaffold, the 3D scaffold of the present invention with co-aligned nanofibers and macrochannels can capture more adherent and non-adherent cells. More interestingly, the scaffold not only significantly promotes cell proliferation, but also induces human umbilical vein endothelial cells (HUVECs) to assemble into blood vessel-like structures, as well as 3D proliferation of embryonic dorsal root ganglion neurons (DRG) and neurites.
[0150] Example 2. Formation of 3D structures with co-aligned nanofibers and macrochannels During the initial freezing in liquid nitrogen, silk fibroin (SF) molecules assembled among fine ice crystals were radially oriented (Fig. 2a). After removing the ice crystals in the frozen samples by freeze-drying, a 3D SF scaffold, i.e., AFb scaffold with radially aligned nanofibers and uniformly distributed nanoparticles (Fig. 2b), was obtained (see Fig. 10a). In the following tests, the radially aligned 3D nanofiber scaffold without channels before post-treatment in ethanol is denoted as AFb (A, F and b stand for “aligned”, “nanofibres” and “before post-treatment in ethanol”, respectively). Obviously, the as-prepared SF nanofibers exhibited smooth morphology and were well aligned radially (see Fig. 10a). The method is facile and allows for the fabrication of samples with various shapes (including tubes and particles), diameters and thicknesses (see Fig. 10b). Furthermore, the alignment direction of the scaffold nanofibers can be controlled by directionally freezing the SF solution in liquid nitrogen (see Figure 10b). For example, vertically aligned nanofibers can be fabricated by slowly lowering a tube containing the SF solution into liquid nitrogen. Particles with radially aligned nanofibers were obtained by directly dropping the SF solution into liquid nitrogen. Furthermore, dropping or spraying a solution containing fiber-forming molecules (silk fibroin) into liquid nitrogen produced particles or spheres with radially aligned nanofibers similar to those in Figure 10b.
[0151] We have shown that rapid freezing and high temperature difference are beneficial for the formation of nanofibers and directional structures. Instead of using liquid nitrogen for flash freezing, we froze the SF solution contained in the same glass tube in a freezer at -80°C and -20°C, respectively, and then used freeze-drying to remove the ice crystals. The SF scaffold obtained from -80°C freezing has a hybrid structure with random short channel-like structures, pores and nanofibers, but these structures are not interconnected (see Figure 11a). (In the following tests, the hybrid 3D SF scaffold obtained from -80°C freezing before post-treatment in ethanol is denoted as W&Fb, where W represents the walls of the channels and pores, F represents the nanofibers, and b indicates before post-treatment in ethanol. After post-treatment in ethanol, the scaffold is denoted as W&F.)
[0152] In comparison, only random pores are found in the SF scaffold obtained from -20°C freezing, and the pores are not well connected to form a network (see also Fig. 11b). Decreasing the freezing rate and temperature difference may promote the growth of random and large ice crystals and the formation of large but non-interconnected pores, so that the scaffold has a wall-like structure. In the following tests, the porous wall-like 3D scaffold obtained from -20°C freezing before post-treatment in ethanol is denoted as Wb, where W represents the walls of pores and b indicates before post-treatment in ethanol. After post-treatment in ethanol, the scaffold is denoted as Wb.
[0153] A second freezing at a relatively low temperature (-20 °C) created macrochannels in the fiber scaffold (Fig. 2c, d). In the 3D micro-CT image (Fig. 3a), each radially aligned channel (100-1000 µm in diameter) connected the surface and center of the scaffold. As shown by SEM (Fig. 3b), the channel walls are composed of SF nanoparticles and nanofibers (50-600 nm in diameter) aligned along the channel direction (indicated by the large yellow arrow). Zooming in on a representative channel wall revealed many pores (50-1000 nm in diameter) that appear to be aligned with the nanofiber orientation.
[0154] In the following tests, these kinds of 3D SF scaffolds with radially aligned nanofibers and channels are denoted as A(F&C) (Fig. 2d). Here, A stands for "radially aligned", F stands for nanofibers, and C stands for channels. More interestingly, a central channel (0.4-2 mm in diameter) was created from the top to the bottom of the scaffold (Fig. 2d, digital photo of A(F&C) scaffold). All relevant sizes within the hierarchical 3D A(F&C) scaffold were summarized in Fig. 3c. Interestingly, A(F&C) scaffolds derived from not only SF but also other mixtures such as SF / gelatin and other biopolymers such as sodium alginate can be prepared using the method of the present invention (see Fig. 12). In comparison, there was no noticeable change after treating Wb and W&Fb scaffolds with the same post-treatment. The pores or short channel-like structures of both scaffolds appeared to be non-interconnected (in the following studies, the 3D Wb and W&Fb scaffolds after post-treatment in ethanol using the above procedure are denoted as W and W&F, respectively) (see Figures 13 and 14 for W&F and W scaffolds).
[0155] Example 3. Secondary structure and mechanical properties of scaffolds To understand the effect of the preparation method on the structural changes of silk fibroin, the secondary structure of the scaffolds was investigated. The conformational changes of SF were observed by the characteristic absorption peaks in the ATR-FTIR spectrum (amide II at 1600–1500 cm -1 , amide I is 1700-1600 cm -1 ) shift. Before post-treatment with ethanol, all three scaffolds had a shift of approximately 1644 cm, suggesting a random coil. -1 The Wb and W&Fb scaffolds showed one major characteristic peak at 1517 cm -1 (indicating a major β-sheet structure), whereas the AFb scaffold showed another major characteristic peak at 1533 cm -1 (indicating a predominant random coil structure), suggesting that low-temperature treatment with liquid nitrogen may be beneficial for the formation of random coils (see FIG. 15a). After treatment in ethanol, all three scaffolds showed distinct peaks at approximately 1700, 1622 and 1517 cm. -1 showed a major characteristic peak at 100 nm, suggesting that the treated scaffolds were mainly composed of β-sheet structures (see Figure 15b).
[0156] The compressive modulus of the scaffolds was shown in Figure 16a. The 3D A(F&C) nanofiber scaffolds had a compressive modulus of about 80 kPa, which is lower than that of the wall-like W and W&F scaffolds (about 100 and about 140 kPa, respectively). This may be due to their large channel-based structure with nanofibers. Of note, after being compressed in mechanical testing, the A(F&C) scaffolds still maintained good radially aligned morphology and structure, and their surfaces showed slight collapse, possibly due to the damage of some channels (see Figure 16b).
[0157] Example 4. Co-aligned channels and nanofibers promote cell entrapment and guide adherent human umbilical vein endothelial cell (HUVEC) proliferation, behavior, and function within 3D SF scaffolds. To understand the effect of the aligned channels and nanofibers on cells, classically adherent HUVECs were used to investigate the ability of the scaffolds to capture cells and promote their proliferation. At both time points, the A(F&C) scaffolds showed significantly higher cell capture and proliferation abilities than the W and W&F scaffolds, indicating that the aligned channels and nanofiber structure of the A(F&C) scaffolds were beneficial for cell adhesion and proliferation (Figure 6a, b). Compared with the W scaffold, the W&F scaffolds showed higher cell adhesion at 8 hours and proliferation viability at 6 days, which was probably due to the presence of nanofibers in the W&F scaffolds.
[0158] To further identify the influence of channels, the AFb scaffold after post-treatment in ethanol (i.e., the AF scaffold in Figure 6) was used as a cell culture substrate. Without the second freezing step and freeze-drying, the AF scaffold had the same radially aligned nanofiber structure as the AFb scaffold shown in Figure 2 and Figure 10a, but did not have channels as shown in the A(F&C) scaffold. The A(F&C) scaffold showed significantly higher cell viability than the AF scaffold at both time points, indicating the advantage of channels for cell capture and proliferation. In addition, the W and W&F scaffolds also showed higher cell viability than the AF scaffold. This is probably due to the fact that the W, W&F and A(F&C) scaffolds provide more space for cell adhesion and proliferation due to their relatively large pores or channels.
[0159] To gain more insight into the effects of aligned channels and nanofibers, confocal fluorescence microscopy was used to image cells grown within the scaffolds for 3 days (Figure 6d). To date, issues remain that cellular behaviors, including cell spreading, migration, elongation, and interaction, are often hindered due to the small pores, and low interconnectivity of the scaffolds, as well as the lack of binding and guidance cues within the scaffolds. This is true for both W and W&F scaffolds. As shown in Figure 6d, cell spreading was notably restricted by the pore walls (indicated by yellow arrows in W) or showed smooth edges (indicated by white arrows in W&F) as if the cells were cultured on the surface of a flat material. Cells were also observed in the AF scaffolds (Figure 6d), but due to the low cell numbers in the inner (internal) region of the scaffolds, it was difficult to find them during scanning under the confocal microscope. The cells in the AF scaffolds were not well aligned or elongated in the direction of the nanofibers, and showed a relatively flat and polygonal morphology. This is probably due to the fact that the loosely aligned nanofibers provide many surrounding signals to the cells from various directions. The cells on the walls of the A(F&C) scaffold were well elongated and aligned along the nanofibers. The presence of large 3D channels reduces the space within the scaffold such that the nanofibers are compressed onto the channel walls, providing the cells with relatively more signals in the long axis (longitudinal) direction of the nanofibers (the directions of the channels and nanofibers are indicated by white arrows, respectively). This may explain the cell proliferation and morphology observed on the A(F&C) scaffold.
[0160] In vascular development and angiogenesis, the proliferation, migration and interaction of endothelial cells are very important for the formation of tube structures. HUVEC is a classical endothelial cell model for testing angiogenesis. As mentioned above, A(F&C) scaffolds can promote the proliferation of HUVEC. It is believed that the cell migration and elongation induced by the aligned channels and nanofibers enhances cell-cell interactions to promote the formation of vessel-like structures. To demonstrate this, we cultured HUVEC for up to 21 days to observe the angiogenic behavior of the cells within the scaffold (Figure 7, Figure 6c shows how to read the image). All cells were CD31 positive (CD31 is a glycoprotein expressed on endothelial cells), suggesting that they maintained the characteristics of HUVEC within the scaffold even after long-term culture.
[0161] In the W and W&F scaffolds, most cells maintained a round morphology and only a few nuclei were elongated (Fig. 7a). Cell spreading, migration and elongation were restricted by the scaffold walls, resulting in localized aggregation and interaction of some cells. In the AF scaffold, some cell nuclei were elongated, but most cells were not significantly aligned or elongated and exhibited polygonal morphology (Fig. 7a). Interestingly, in the A(F&C) scaffold, all cells and cell nuclei were elongated and aligned on the channel walls, interacted on the channel walls and assembled into CD31-positive vessel-like structures (the channel, channel walls, vessel-like structures and aligned and elongated cell nuclei are indicated by white arrows, respectively) (Fig. 7a). Fourteen consecutive confocal slices of the channel in Fig. 7a are shown in Fig. 7b. Inside the A(F&C) scaffold, there were many vessel-like structures aligned on the channel walls. These findings demonstrated that the co-aligned channels and nanofibers enhanced the spreading, migration, elongation and interaction of HUVECs to assemble into vessel-like structures.
[0162] Example 5. Co-aligned channels and nanofibers enhance scaffold capture for non-adherent embryonic dorsal root ganglion neurons (DRG) and induce 3D outgrowth of neurites within the scaffold. Non-adherent DRGs were used to further confirm the effects of the co-aligned channels and nanofibers on cells. As shown in Figure 8a, the A(F&C) scaffold also exhibited excellent DRG capture ability. The AF scaffold showed the lowest DRG capture, and no significant difference was observed between the W and W&F scaffolds. These observations suggest that the co-aligned channels and nanofibers of the scaffolds may be useful for capturing not only adherent cells but also non-adherent cells. Figure 8b shows the scanned areas of the scaffolds and the corresponding images. Abundant neurites were aligned in the direction of the nanofibers on the surface of the AF scaffold, but were not observed in the inner part of the scaffold. In the macroporous W and W&F scaffolds, the neurites were aggregated only on the surface. These results indicated that in the absence of channels, it was difficult for DGRs to grow into the inner region of the scaffold during 21 days of culture, and the neurite outgrowth of DRGs was inhibited.
[0163] Figure 8c shows the scanned area and corresponding images of the A(F&C) scaffold. The DRG could be clearly seen, and a significant amount of long neurites had grown through the channel (the channel, channel wall, and neurites were indicated by white arrows, respectively). Interestingly, a magnification of the channel revealed that both the DRG and neurites grew mainly along the channel, suggesting a 3D growth mode of the neurites. This was quite different from the 2D growth of the DRG and neurites along the aligned nanofibers on the surface of the AF scaffold (Figure 8b). From the last image in Figure 8c, bundled neurites were clearly observed, which are very important for the formation of neural tissue. These observations demonstrated that the aligned channels and nanofibers could not only promote the adhesion and proliferation of both adherent and non-adherent cells, but also induce them to proliferate, migrate, and interact in 3D space similar to the natural ECM.
[0164] At present, 3D scaffolds with mainly wall-like porosity have been the most studied so far. Despite the tunable pore size, the low interconnectivity of pores within the scaffolds limits cell and tissue infiltration, migration and proliferation as well as the transport of oxygen, nutrients and waste products. Figure 17 provides insight into DRG proliferation within various porous scaffolds after 21 days of culture. In the W scaffold, neurite invasion of aggregated DRGs occurred only along the pore walls. In the W&F scaffold, the pore walls caused the aggregation of DRGs and restricted neurite outgrowth. In the A(F&C) scaffold, radially aligned channels (100-1000 μm in diameter) toward the center of the scaffold provided sufficient space for cell migration and 3D proliferation, as shown in Figure 6d, Figure 7a, b and Figure 8c.
[0165] A common problem in tissue engineering is the necrosis of cells or tissues within the 3D scaffold due to insufficient supply of oxygen and nutrients. The channels with porous walls (pore size 50-1000 nm) within the A(F&C) scaffold are crucial for the transport of oxygen, nutrients and waste products. The large central channel (diameter 0.4-2 mm) of the scaffold should also facilitate nutrient exchange and waste disposal.
[0166] The aligned nanofibers (50-600 nm in diameter) on the channel walls played an important role in cell capture, proliferation, and guiding cells to migrate and proliferate along the aligned direction (Figure 6a, b, d, Figure 7a, b, and Figure 8a). In addition, the nanofibers and nanoparticles are excellent carriers for the delivery of growth factors or drugs. As shown in Figure 7a and Figure 8c, the channels showed good morphology and structure even after 21 days of cell culture, indicating the stability of the scaffold.
[0167] The A(F&C) scaffold was developed as a proof-of-concept model platform that the creation of ECM-mimicking 3D structures plays a key role in insights into cell behavior and function in vitro. Based on this platform, we discovered that adherent HUVECs preferred to grow along the material within the 3D scaffold. Thus, adherent HUVECs were mainly guided by the aligned nanofibers on the walls of the A(F&C) scaffold (Fig. 9a, b). In contrast, non-adherent DRG and neurites preferred to grow along the 3D space. As shown in Fig. 9c, d, e, neurites mainly grew along the channels. However, on the 2D surface of the AF scaffold, neurites were highly aligned in the direction of the aligned nanofibers (Fig. 8b). Considering the facile fabrication technique, the findings in this study will pave the way for developing a new kind of 3D scaffold based on aligned nanofibers and channels for use in tissue engineering. For example, creating nanofiber tube scaffolds with radially aligned channels using biocompatible polymers could be beneficial for multi-layered cell seeding. Similarly, constructing a pillar scaffold containing channels aligned along the long axis (lengthwise) of the scaffold could provide better support for nerve regeneration than hollow tubes with thin walls.
[0168] Therefore, we developed a facile freeze-drying strategy to create a biomimetic 3D scaffold with aligned nanofibers and macrochannels. As a model platform for in vitro cell culture and testing, the 3D scaffold showed significantly higher cell capture and proliferation promotion capacity for both adherent HUVECs and non-adherent DRG than the widely used non-channel wall-like 3D scaffolds and 3D aligned nanofiber scaffolds. More importantly, the aligned nanofibers and channels not only induce the proliferation, migration and interaction of HUVECs to assemble into vessel-like structures within the scaffolds in vitro, but also induce the neurite outgrowth of DRG in the 3D space.
[0169] Those skilled in the art will appreciate that the invention described herein may be susceptible to variations and modifications other than those specifically described, and it is to be understood that the invention includes all such variations and modifications that are within the spirit and scope of the invention.
Claims
1. A method for manufacturing a nanofiber-based nanotube device, comprising: said macrochannels having diameters between 100 μm and 1000 μm and interconnected by linear or radial alignments of said nanofibers to define a three-dimensional matrix; the channel walls include a plurality of pores between the nanofibers, the pores having diameters between 20 nm and 800 nm; The nanofibers have a diameter between 20 nm and 5000 nm and are a porous biomimetic scaffold comprising one or more polymers selected from natural polymers, synthetic polymers, or combinations thereof.
2. 10. The porous biomimetic scaffold of claim 1 comprising nanoparticles dispersed along the nanofibers of the nanofiber wall.
3. 3. The porous biomimetic scaffold of claim 2, wherein the nanoparticles are formed of at least one natural polymer selected from the group consisting of silk fibroin, alginate, bovine serum albumin, collagen, chitosan, gelatin, sericin, hyaluronic acid, and starch.
4. A porous biomimetic scaffold according to any one of claims 1 to 3, wherein the aligned nanofibers have a length of at least 50 nm and a diameter of 50 nm to 600 nm, and the pores have a diameter of 20 nm to 500 nm.
5. 5. The porous biomimetic scaffold of any one of claims 1 to 4, wherein the aligned nanofibers are formed of at least one natural polymer selected from the group consisting of silk fibroin, alginate, bovine serum albumin, collagen, chitosan, gelatin, sericin, hyaluronic acid, and starch.
6. 5. The porous biomimetic scaffold according to any one of claims 1 to 4, wherein the aligned nanofibers are formed of at least one synthetic polymer selected from the group consisting of vinyl polymers, poly(ethylene oxide), polyformaldehyde, polyacetaldehyde, poly(3-propionate), poly(10-decanoate), poly(ethylene terephthalate), polycaprolactam, poly(11-undecanoamide), poly(hexamethylene sebacamide), poly(m-phenylene terephthalate), poly(tetramethylene-m-benzenesulfonamide) and copolymers thereof.
7. 7. The porous biomimetic scaffold of any one of claims 1 to 6, further comprising at least one additive selected from the group consisting of drugs, growth factors, polymers, surfactants, chemicals, particles, porogens and combinations thereof.
8. 8. The porous biomimetic scaffold of claim 1, further comprising at least one adjuvant selected from surfactants, preservatives, wetting agents, emulsifiers and dispersing agents.
9. The porous biomimetic scaffold of claim 1 , wherein the aligned nanofibers are crosslinked.
10. 10. The porous biomimetic scaffold according to any one of claims 1 to 9, having a compressive modulus of 20 to 160 kPa.
11. A biomedical implant comprising a porous biomimetic scaffold according to any one of claims 1 to 10.
12. 11. Use of the porous biomimetic scaffold according to any one of claims 1 to 10 for trapping and culturing cells in vitro to promote cell proliferation.
13. 11. Use of a biomedical implant comprising a porous biomimetic scaffold according to any one of claims 1 to 10 as an in vitro cell carrier template for cell culture, tissue repair and / or tissue engineering.
14. A porous biomimetic scaffold described in any one of claims 1 to 10 or a biomedical implant described in claim 11 for the treatment of tissue damage.
15. A porous biomimetic scaffold as described in any one of claims 1 to 10 or a biomedical implant as described in claim 11 for use in the treatment of a mammal having suffered tissue damage and in need of tissue repair and / or regeneration.
Citation Information
Patent Citations
Manufacturing method of porous structure
JP2001524596A
Transplantable material and method for preparing the same
JP2011521020A
Implantable intervertebral disc devices and uses thereof
US20140222152A1
Silk-based scaffold platform for engineering tissue constructs
US20170027879A1