Polyurethane-based pressure-sensitive adhesive composition, surface protection film including same, method for manufacturing surface protection film, and method for manufacturing organic light-emitting electronic device

A polyurethane adhesive composition with controlled bifunctional and trifunctional polyol ratios addresses adhesion and removability issues in surface protection films, ensuring effective protection and easy removal without residue, even at high temperatures.

JP7566356B2Active Publication Date: 2024-10-15XINMEI HOLDINGS (HONG KONG) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022559710
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-07
Filing Date
2021-09-07
Publication Date
2024-10-15
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

Existing surface protection films for flexible displays face challenges with adhesive compositions that either fail to adhere well, cause damage, or leave residue, and do not maintain adhesion at high temperatures, while also being difficult to remove without contamination.

Method used

A polyurethane pressure-sensitive adhesive composition is developed, comprising specific ratios of bifunctional and trifunctional polyols and an isocyanate crosslinking agent, with controlled viscosity and crosslink density, ensuring excellent adhesion, removability, and resistance to temperature changes.

Benefits of technology

The composition provides good adhesion to substrates, prevents damage and contamination, maintains adhesion at high temperatures, and allows easy removal with minimal residue, enhancing the protection of flexible displays during manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566356000003
    Figure 0007566356000003
  • Figure 0007566356000004
    Figure 0007566356000004
  • Figure 0007566356000001
    Figure 0007566356000001
Patent Text Reader

Abstract

The present invention relates to a polyurethane-based pressure-sensitive adhesive composition, a surface protection film containing the same, a method for producing a surface protection film, and a method for producing an organic light-emitting electronic device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2020-0113642, filed with the Korean Intellectual Property Office on September 7, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a polyurethane-based pressure-sensitive adhesive composition, a surface protection film containing the same, a method for producing a surface protection film, and a method for producing an organic light-emitting electronic device. [Background technology]

[0003] In recent years, with the development of display-related technologies, display devices that can be transformed during use, such as by folding, rolling into a roll, stretching like a rubber band, etc., have been researched and developed. These displays can be transformed into various shapes, so they can meet both the demand for larger displays during use and the demand for smaller displays for portability.

[0004] Furthermore, in recent years, portable terminals such as wireless terminals, personal digital assistants (PDAs), portable multimedia players (PMPs), electronic organizers, etc. tend to become smaller in size for the sake of portability.

[0005] However, since users want to receive information from various contents such as text information, videos, games, etc. through the screen of a mobile terminal, they are demanding larger or wider display screens. However, the miniaturization of a mobile terminal leads to a reduction in the size of the display screen, so there is a limit to satisfying both of these requirements.

[0006] Conventionally, unbreakable displays have been used as display devices. However, in order to overcome the above limitations, deformable displays, i.e. flexible displays such as curved displays, bent displays, foldable displays, and rollable displays, have been developed.

[0007] Plastic substrates used as substrate materials for flexible displays have a problem in that they have extremely low barrier properties against gases such as moisture and oxygen. To address this problem, barrier films made of various materials and structures were formed on the substrate to improve the plastic substrate problem.

[0008] However, in recent years, as existing barrier films are no longer used, there is a demand for the development of process surface protection films that can protect the thin film encapsulation (TFE) layer during the manufacturing process of flexible optical elements. The process surface protection film is a film that temporarily protects the thin film encapsulation layer, and is attached to the thin film encapsulation layer during processing to prevent contamination and damage to the surface of the thin film encapsulation layer during processing, and is removed when the processing is completed.

[0009] The physical properties required for the surface protection film are, first, that the adhesive provided in the surface protection film should adhere well to the surface of the adherend, that the adhesive should be removable with a low peeling force in the removal step, and that the damage to the adherend should be prevented, and, second, that the adhesive residue should be small after the surface protection film is removed, and that the contamination of the adherend should be prevented.

[0010] Generally, examples of adhesives used in surface protection films include acrylic, silicone, and urethane adhesives. Acrylic adhesives have excellent adhesive strength, but poor removability after adhesion, which may damage the adherend or leave residue on the adherend, while silicone adhesives have excellent low-speed and high-speed peel strength after adhesion to the adherend, but are prone to contaminating the adherend.

[0011] Therefore, in order to solve these problems, it is necessary to develop a novel pressure-sensitive adhesive composition and a protective film containing the same. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Japanese Patent Publication No. 2006-299283 Summary of the Invention [Problem to be solved by the invention]

[0013] The present application provides a polyurethane-based pressure-sensitive adhesive composition, a surface protection film containing the same, and a method for producing the same. [Means for solving the problem]

[0014] One embodiment of the present application provides a polyurethane-based pressure-sensitive adhesive composition comprising a polyurethane polymer containing a bifunctional polyol and a trifunctional polyol; and an isocyanate-based crosslinking agent, the polyurethane-based pressure-sensitive adhesive composition having a viscosity of 1,000 cPs or more and 10,000 cPs or less under conditions of 25°C and a relative humidity of 60%, and comprising 5 to 40 parts by weight of the bifunctional polyol per 100 parts by weight of the polyurethane polymer, and 60 to 95 parts by weight of the trifunctional polyol per 100 parts by weight of the polyurethane polymer.

[0015] Another embodiment provides a surface protection film comprising: a base film; and an adhesive film comprising the polyurethane-based adhesive composition according to the present application or a cured product thereof provided on one side of the base film.

[0016] Another embodiment provides a method for producing a surface protection film, comprising the steps of: preparing a polyurethane-based pressure-sensitive adhesive composition according to the present application; adding a curing agent to the polyurethane-based pressure-sensitive adhesive composition; and coating the polyurethane-based pressure-sensitive adhesive composition onto a substrate film.

[0017] Finally, another embodiment of the present application provides a method for manufacturing an organic light-emitting electronic device, comprising attaching an adhesive film of a surface protection film according to the present application onto an encapsulation layer of an organic light-emitting device. Effect of the Invention

[0018] In the case of a polyurethane-based pressure-sensitive adhesive composition according to one embodiment of the present application, the content of bifunctional polyol and trifunctional polyol satisfies a specific range, and the hydroxyl group of the urethane polyol can be controlled to effectively adjust the urethane crosslink density.

[0019] In addition, the viscosity of the adhesive composition satisfies a specific range, so that the thickness deviation relative to the substrate during adhesive coating is small, and excellent coating properties can be exhibited.Then, an adhesive film containing the same has good adhesion to the adherend, excellent adhesive strength, and good removability at low speed and also excellent removability at high speed.It has the characteristics of being able to protect the adherend due to its excellent adhesive strength with the adherend during processing, and being able to prevent contamination of the adherend due to the small amount of adhesive film residue when removed.

[0020] In addition, the surface protection film according to one embodiment of the present application has the characteristic that even when the surface protection film is removed from the adherend, only a small amount of adhesive film remains on the surface of the adherend, thereby preventing damage or contamination of the adherend surface after removal of the surface protection film.

[0021] Furthermore, the surface protective film of the present invention maintains its adhesive strength to the adherend even when the temperature rises, and can prevent the surface protective film from lifting off the adherend at high temperatures. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a side view of a surface protection film according to one embodiment of the present application. [Diagram 2] 5 shows an embodiment in which a surface protection film according to an embodiment of the present invention is attached to an organic light emitting device 510. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] This specification will be explained in more detail below. Prior to describing the present invention, some terms will first be defined.

[0024] In this specification, when a part "comprises" a certain component, this does not mean excluding other components, but means that the part may further include other components, unless otherwise specified to the contrary. In this specification, "p to q" means a range of "not less than p and not more than q".

[0025] As used herein, (meth)acrylate includes both acrylate and methacrylate.

[0026] In this specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer participates in a polymerization reaction and is contained as a repeating unit in the polymer. When a polymer contains a monomer in this specification, this is interpreted as being equivalent to saying that the polymer contains the monomer as a monomer unit.

[0027] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless otherwise specified as a "homopolymer." In this specification, the term "monomer unit" refers to a state in which the compound is polymerized and bonded in a polymer.

[0028] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using commercially available monodisperse polystyrene polymers (standard samples) with various degrees of polymerization as standard substances for molecular weight measurement. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0029] The weight average molecular weight is one of the average molecular weights in which the molecular weight of a polymer substance is not uniform and is used as a standard, and is a value obtained by averaging the molecular weights of component molecular species of a polymer compound having a molecular weight distribution by weight fraction. The weight average molecular weight can be measured by gel permeation chromatography (GPC) analysis.

[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.

[0031] One embodiment of the present application provides a polyurethane-based pressure-sensitive adhesive composition comprising a polyurethane polymer containing a bifunctional polyol and a trifunctional polyol; and an isocyanate-based crosslinking agent, the polyurethane-based pressure-sensitive adhesive composition having a viscosity of 1,000 cPs or more and 10,000 cPs or less under conditions of 25°C and a relative humidity of 60%, and comprising 5 to 40 parts by weight of the bifunctional polyol per 100 parts by weight of the polyurethane polymer, and 60 to 95 parts by weight of the trifunctional polyol per 100 parts by weight of the polyurethane polymer.

[0032] In the case of a polyurethane-based pressure-sensitive adhesive composition according to one embodiment of the present application, the content of bifunctional polyol and trifunctional polyol satisfies a specific range, and the hydroxyl group of the urethane polyol can be controlled to effectively adjust the urethane crosslink density.

[0033] In addition, the viscosity of the adhesive composition satisfies a specific range, so that the thickness deviation relative to the substrate during adhesive coating is small, and excellent coating properties can be exhibited.Then, an adhesive film containing the same has good adhesion to the adherend, excellent adhesive strength, good removability at low speed and excellent removability at high speed, and has the characteristics of being able to protect the adherend due to excellent adhesive strength with the adherend during processing, and being able to prevent contamination of the adherend due to little adhesive film residue when removed.

[0034] In one embodiment of the present application, the bifunctional polyol and trifunctional polyol are particularly preferably ether polyols. In one embodiment of the present application, the polyurethane polymer may contain 5 to 40 parts by weight of a bifunctional polyol relative to 100 parts by weight of the polyurethane polymer, and 60 to 95 parts by weight of a trifunctional polyol relative to 100 parts by weight of the polyurethane polymer.

[0035] In one embodiment of the present application, the polyurethane polymer may contain 5 to 40 parts by weight, preferably 7 to 35 parts by weight, and more preferably 10 to 30 parts by weight of a bifunctional polyol based on 100 parts by weight of the polyurethane polymer. In one embodiment of the present application, the polyurethane polymer may contain 60 to 95 parts by weight, preferably 60 to 90 parts by weight, and more preferably 70 to 90 parts by weight of a trifunctional polyol based on 100 parts by weight of the polyurethane polymer.

[0036] The polyurethane-based pressure-sensitive adhesive composition according to the present application has a polyurethane polymer, and in particular the bifunctional polyol and trifunctional polyol in the polyurethane polymer satisfy the above-mentioned weight ranges. In particular, when the bifunctional polyol satisfies the above-mentioned weight range, it has the characteristics of imparting two-dimensional crosslinking and subsequent adhesion and flexibility to the adherend, and having an appropriate crosslinking distance and peeling force. In contrast, when the trifunctional polyol satisfies the above-mentioned weight range, it has the characteristics of increasing the degree of three-dimensional crosslinking to reduce the re-peeling force, and adjusting the molecular weight range to a specific range to prevent gelation of the pressure-sensitive adhesive composition containing it.

[0037] In one embodiment of the present application, there is provided a polyurethane-based pressure-sensitive adhesive composition, wherein the polyurethane polymer has a molar ratio of hydroxyl groups to isocyanate functional groups (-OH / NCO) of 1.3 or more and 1.7 or less.

[0038] In another embodiment, the polyurethane polymer may have a molar ratio of hydroxyl groups to isocyanate functional groups (-OH / NCO) of 1.3 to 1.7, preferably 1.35 to 1.7, more preferably 1.4 to 1.65.

[0039] In this application, a functional group, also referred to as a functional atom group, functional group, or functional group, can refer to a common grouping of atoms or bonding pattern responsible for a common chemical property in a group of organic compounds having that property.

[0040] In other words, in this application, expressions such as bifunctional and trifunctional refer to the number of functional groups having common chemical properties in a particular molecule, and specifically, bifunctional may mean having two functional groups, and trifunctional may mean having three functional groups.

[0041] In this application, polyol is a material obtained by reacting an initiator such as a multifunctional alcohol or aromatic amine having two or more hydroxyl groups (-OH) or amine groups (-NH2) in the molecule with propylene oxide (PO) or ethylene oxide (EO) under specific conditions, and is a raw material for producing polyurethane polymer together with isocyanate. The polyol may refer to a material having two or three functional groups obtained by reacting PPG (propylene glycol), PTMEG (tetramethylene glycol), PEG (ethylene glycol) Polyester with propylene oxide (PO) or ethylene oxide (EO).

[0042] In the present application, the ratio of functional groups of the polyurethane polymer satisfies the above range, so that the pressure-sensitive adhesive composition can be prevented from gelling, and the molecular weight and viscosity ranges can be appropriately adjusted, so that the pressure-sensitive adhesive composition has characteristics suitable for coating. That is, in one embodiment of the present application, the ratio of functional groups of the polyurethane polymer is adjusted to have a suitable molecular weight and viscosity, and the adjustment factor is the content and type of the solvent or crosslinker contained in the pressure-sensitive adhesive composition.

[0043] In one embodiment of the present application, the pressure-sensitive adhesive composition may have a viscosity of 1,000 cPs or more and 10,000 cPs or less under conditions of 25° C. and a relative humidity of 60%.

[0044] In this application, viscosity is a quantity that indicates the degree of difficulty in the flow of a fluid, that is, the degree of stickiness. When a fluid flows, the shear force per unit area acting between adjacent fluid layers is proportional to the velocity gradient at that position, and this proportionality constant can be called viscosity. That is, in this application, viscosity is the internal resistance when a fluid flows, and methods of expressing viscosity include kinetic viscosity and absolute viscosity.

[0045] In one embodiment of the present application, the viscosity can be measured by measuring the viscosity of a liquid sample having a low to high viscosity at a constant temperature using a Brookfield HB type rotational or vibration type viscometer.

[0046] Specifically, the viscosity can be measured using a Brookfield viscometer (Brookfield HB) at a temperature of 25° C. using a Brookfield No. 40 and No. 52 spindle. In this case, the rotation speed can be adjusted so that the torque value, which is the force applied to the composition, is between 20% and 60%.

[0047] In one embodiment of the present application, the viscosity of the pressure-sensitive adhesive composition may be in the range of 1,000 cPs or more and 10,000 cPs or less, preferably 1,500 cPs or more and 8,000 cPs or less, more preferably 2,000 cPs or more and 7,000 cPs or less, under conditions of 25° C. and a relative humidity of 60%.

[0048] In the present application, when the viscosity of the pressure-sensitive adhesive composition is outside the above-mentioned lower limit range, the pressure-sensitive adhesive composition flows during subsequent coating, making coating difficult, and when the viscosity is outside the above-mentioned upper limit range, it is difficult to pump the coating liquid during mass production, reducing the productivity of the pressure-sensitive adhesive film.

[0049] In one embodiment of the present application, the viscosity basically increases as the molecular weight increases, and the viscosity value increases as the ratio of trifunctional polyol contained in the pressure-sensitive adhesive composition increases. Ultimately, the polyurethane-based pressure-sensitive adhesive composition according to the present application has the above-mentioned viscosity range and the below-described molecular weight range achieved by the bifunctional polyol and trifunctional polyol in the polyurethane polymer satisfying the above-mentioned specific weight range and the functional group ratio (-OH / NCO) satisfying a specific range, thereby achieving the main object of the present invention.

[0050] In one embodiment of the present application, there is provided a pressure-sensitive adhesive composition, in which the polyurethane polymer contains a solvent, and the solvent is contained in an amount of 5 parts by weight or more and 35 parts by weight or less per 100 parts by weight of the total of the bifunctional polyol and the trifunctional polyol.

[0051] The solvent contained in the polyurethane polymer may be toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), or ethyl acetate (EAc). However, the solvent is not limited thereto and any general organic solvent may be used as long as it can dissolve a specific substance.

[0052] In another embodiment, the polyurethane polymer may contain a solvent and may contain 5 parts by weight or more and 35 parts by weight or less, preferably 7 parts by weight or more and 35 parts by weight or less, and more preferably 10 parts by weight or more and 30 parts by weight or less, per 100 parts by weight of the total of the bifunctional polyol and the trifunctional polyol.

[0053] The ratio of functional groups in the polyurethane polymer is adjusted to have a suitable molecular weight and viscosity, and the adjustment factors depend on the content and type of the solvent or crosslinking agent contained in the pressure-sensitive adhesive composition. In particular, by adjusting the range of the solvent content in the production of the polyurethane polymer as described above, the viscosity of the pressure-sensitive adhesive composition itself can be adjusted to a specific range, resulting in excellent productivity and the ability to prevent gelation.

[0054] In one embodiment of the present application, the non-volatile content of the polyurethane polymer may be in the range of 65% to 95%. In another embodiment, the non-volatile content of the polyurethane polymer may be from 65% to 95%, from 70% to 95%, or from 75% to 90%.

[0055] In one embodiment of the present application, there is provided a pressure-sensitive adhesive composition, wherein the molecular weight of the polyurethane polymer is 50,000 g / mol or more and 200,000 g / mol or less. In another embodiment, the molecular weight of the polyurethane polymer may satisfy the range of 50,000 g / mol to 200,000 g / mol, preferably 60,000 g / mol to 180,000 g / mol, more preferably 80,000 g / mol to 150,000 g / mol.

[0056] When the molecular weight of the polyurethane polymer satisfies the above range, the viscosity of the pressure-sensitive adhesive composition containing the polyurethane polymer satisfies a specific range, resulting in excellent productivity and the ability to prevent gelation.

[0057] That is, in the case of the polyurethane-based adhesive composition according to the present application, the content of the bifunctional polyol and the trifunctional polyol meets a specific range, and the viscosity of the adhesive composition meets a specific range, so that the adhesive film containing it has good adhesion to the adherend, excellent adhesive strength, and good removability at low speed and excellent removability at high speed. In addition, the adhesive strength with the adherend is excellent during the process, so that the adherend can be protected, and the adhesive film residue is small when removed, so that contamination of the adherend is prevented, and in terms of the production of the polyurethane polymer, it has the characteristics of preventing gelation, excellent coating properties, and excellent productivity.

[0058] In one embodiment of the present application, the polyurethane-based pressure-sensitive adhesive composition may have a glass transition temperature (Tg) value of 0° C. or lower, or −60° C. or higher, preferably −50° C. or higher.

[0059] In one embodiment of the present application, the glass transition temperature of the polyurethane-based pressure-sensitive adhesive composition may satisfy the above range by adjusting the molar ratio (content ratio) of the polyurethane polymer and the isocyanate-based crosslinking agent contained in the pressure-sensitive adhesive composition.

[0060] The adhesive composition according to the present application has a glass transition temperature value that satisfies the above range, and thus the adhesive film containing the adhesive composition has a feature of being particularly excellent in folding properties. That is, in the case of the adhesive composition according to the present application, by adjusting the molar ratio (content ratio) of the polyurethane polymer and the isocyanate-based crosslinking agent contained in the adhesive composition to a specific range, the glass transition temperature of the entire adhesive composition can be adjusted to a range of 0°C or less, and thus an adhesive film having particularly excellent folding and bending properties can be formed.

[0061] In this specification, the glass transition temperature is a value measured by using a differential scanning calorimeter (DSC, Mettler) to seal about 10 mg of a sample in a dedicated pan and heat it in a constant temperature environment, and plotting the amount of heat absorption and heat generation of the substance that accompanies a phase transition as a function of temperature.

[0062] Specifically, the glass transition temperature is a nominal value given in literature, catalogs, etc., or a value calculated based on the following general formula 1 (Fox formula). [General formula 1] 1 / Tg=W1 / Tg1+W2 / Tg2+…+Wn / Tgn

[0063] In the general formula 1, Tg represents the glass transition temperature (unit: K) of polymer A, Tgi (i=1, 2, ..., n) represents the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i=1, 2, ..., n) represents the mass fraction of monomer i in the total monomer components. The above general formula 1 means a calculation formula when polymer A contains n kinds of monomer components, namely monomer 1, monomer 2, . . . , monomer n. The above formula 1 is for an acrylic resin based on an acrylic monomer, but it may be similarly measured for a urethane resin as in the present invention, such as the glass transition temperature of a known polyol.

[0064] In one embodiment of the present application, the glass transition temperature of the pressure-sensitive adhesive composition can be estimated by component analysis to estimate the content of each monomer, and the glass transition temperature can be calculated based on the general formula 1 (Fox formula).

[0065] In one embodiment of the present application, there is provided a pressure-sensitive adhesive composition, wherein the polyurethane-based pressure-sensitive adhesive composition further comprises one or more selected from the group consisting of a solvent, a curing agent, a dispersing agent, a photoinitiator, a thermal initiator, a silane coupling agent, a plasticizer, a tackifier, and an antistatic agent.

[0066] In one embodiment of the present application, the crosslinking agent may include a crosslinkable compound, and as the crosslinking agent, an isocyanate-based crosslinking agent or one well known in the art may be used.

[0067] The isocyanate crosslinking agent may be selected from any suitable polyfunctional isocyanate compound commonly used in the art, so long as it is a compound that can be used in a urethane reaction.

[0068] Examples of the polyfunctional isocyanate compound that can be used include, but are not limited to, polyfunctional aliphatic isocyanates, polyfunctional alicyclic isocyanates, polyfunctional aromatic isocyanate compounds, trimethylolpropane adducts obtained by modifying polyisocyanates with trifunctional isocyanates, biuret bodies obtained by reacting polyisocyanates with water, and trimers having an isocyanurate ring.

[0069] Examples of the polyfunctional aliphatic isocyanate compound include, but are not limited to, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0070] Examples of the polyfunctional alicyclic isocyanate compound include, but are not limited to, isophorone diisocyanate (IPDI), 1,4-cyclohexane diisocyanate (CHDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), bis(isocyanatomethyl)cyclohexane (HXDI), and the like.

[0071] Examples of the polyfunctional aromatic isocyanate compound include, but are not limited to, toluene 2,4-diisocyanate (TDI), toluene 2,6-diisocyanate (TDI), 4,4'-methylene diphenyl diisocyanate (MDI), 2,4'-methylene diphenyl diisocyanate (MDI), polymeric methylene diphenyl diisocyanate (PMDI), p-phenylene diisocyanate (PDI), m-phenylene diisocyanate (PDI), naphthalene 1,5-diisocyanate (NDI), naphthalene 2,4-diisocyanate (NDI), p-xylylene diisocyanate (XDI), and 1,3-bis(1-isocyanato-1-methylethyl)benzene (TMXDI).

[0072] In one embodiment of the present specification, the pressure-sensitive adhesive composition may be used by mixing two or more kinds of isocyanate compounds, and in this case, the type and content of the two or more kinds of isocyanate compounds may be appropriately selected.For example, the isocyanate compound contained in the pressure-sensitive adhesive composition may be used by mixing a polyfunctional aromatic isocyanate compound and a polyfunctional aliphatic isocyanate compound.

[0073] The antistatic agent may be a known substance for achieving a desired effect, or may be an appropriate antistatic composition in consideration of the object of the present application, for example, one selected from the group consisting of acrylic resins, urethane resins, urethane-acrylic copolymers, ester resins, ether resins, amide resins, epoxy resins, and melamine resins, or a mixture thereof, but is not limited thereto.

[0074] In one embodiment, the antistatic composition may include a conductive material, which may include, but is not limited to, a conductive polymer or a carbon nanotube.

[0075] The conductive polymer may include, for example, polyaniline, polypyrrole, polythiophene, derivatives or copolymers thereof, but is not limited thereto.

[0076] The carbon nanotube may have a tubular shape formed by rolling up a graphite plate formed of hexagonal rings each having six carbon atoms. The carbon nanotube has excellent rigidity and electrical conductivity, and when it is contained in the antistatic composition of the surface protective film, the hardness can be increased and the antistatic function can be improved. The thermal initiator may be any of those well known in the art.

[0077] The solvent may be toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), or ethyl acetate (EAc). However, the solvent is not limited thereto and any general organic solvent may be used as long as it can dissolve a specific substance.

[0078] In one embodiment of the present application, there is provided a surface protection film comprising: a base film; and an adhesive film comprising the polyurethane-based adhesive composition or a cured product thereof provided on one surface of the base film.

[0079] In the present application, the meaning of a pressure-sensitive adhesive film containing the polyurethane-based pressure-sensitive adhesive composition may include containing the pressure-sensitive adhesive composition as is. In the present application, the meaning of a pressure-sensitive adhesive film containing the polyurethane-based pressure-sensitive adhesive composition may include a film containing the pressure-sensitive adhesive composition in a dried state.

[0080] In the present application, the meaning of a pressure-sensitive adhesive film including the polyurethane-based pressure-sensitive adhesive composition may include a film including the pressure-sensitive adhesive composition after being thermally cured. In the present application, the meaning of a pressure-sensitive adhesive film including the polyurethane-based pressure-sensitive adhesive composition may include a pressure-sensitive adhesive film including the pressure-sensitive adhesive composition after photocuring.

[0081] In one embodiment of the present application, there is provided a surface protection film, which has a low-speed peel force of 5 gf / inch or more when one side of the adhesive film is bonded to a glass substrate and then peeled at a peel angle of 180° and a speed of 1.8 m / min, and has a high-speed peel force of 50 gf / inch or less when one side of the adhesive film is bonded to a glass substrate and then peeled at a peel angle of 180° and a speed of 20 m / min.

[0082] In the present application, the pressure-sensitive adhesive film containing the above-mentioned polyurethane-based pressure-sensitive adhesive composition is characterized by having a good removability at low speed as well as an excellent removability at high speed.

[0083] In another embodiment, when one side of the adhesive film is bonded to a glass substrate and then peeled at a peel angle of 180° and a speed of 1.8 m / min, the low-speed peel force may be 5 gf / inch or more, preferably 5.5 gf / inch or more, and more preferably 6 gf / inch or more.

[0084] In another embodiment, when one side of the adhesive film is bonded to a glass substrate and then peeled at a peel angle of 180° and a speed of 1.8 m / min, the low-speed peel force may be 60 gf / inch or less, preferably 55 gf / inch or less, and more preferably 40 gf / inch or less.

[0085] In another embodiment, after one side of the adhesive film is bonded to a glass substrate, when peeled at a peel angle of 180° and a speed of 20 m / min, the high-speed peel force may be 50 gf / inch or less, preferably 48 gf / inch or less, and more preferably 45 gf / inch or less.

[0086] In another embodiment, after one side of the adhesive film is bonded to a glass substrate, when it is peeled off at a peel angle of 180° and a speed of 20 m / min, the high-speed peel force may be 10 gf / inch or more, preferably 20 gf / inch or more, and more preferably 35 gf / inch or more.

[0087] When the high-speed and low-speed peel strengths of the adhesive film of the present application satisfy the above ranges, the film has good adhesion to the adherend, excellent adhesive strength, and also has good removability at low speed and excellent removability at high speed. The excellent adhesive strength to the adherend during processing can protect the adherend, and the small amount of adhesive film residue left when the film is removed can prevent contamination of the adherend.

[0088] The low speed peel strength refers to a value measured by cutting the adhesive film according to the present invention into a width of 1 inch, adhering it to a glass substrate by rolling it back and forth once with a 2 kg rubber roller, leaving it at 23° C. for 10 minutes or less, and then peeling it at an angle of 180° at a peel speed of 1.8 m / min using a texture analyzer (Stable Micro Systems).

[0089] The high-speed peel strength refers to a value measured by cutting the adhesive film according to the present invention into a width of 1 inch, adhering it to a glass substrate by rolling it back and forth once with a 2 kg rubber roller, leaving it at 23° C. for 10 minutes or less, and then peeling it at an angle of 180° at a peel speed of 20 m / min using a texture analyzer (Stable Micro Systems).

[0090] In one embodiment of the present application, the substrate film may be selected from the group consisting of polyethylene terephthalate (PET), polycarbonate (PC), polyimide (PI), polyethylene naphthalate (PEN), polyether ether ketone (PEEK), polyarylate (PAR), polycylicolefin (PCO), polynorbornene (polynorbornene), polyethersulphone (PES), and cycloolefin polymer (COP). The PET (polyethylene terephthalate), PEN (polyethylene naphthalate), and PAR (polyarylate) may be a type of polyester. In another embodiment, the base film may be made of PET (polyethylene terephthalate).

[0091] In one embodiment of the present application, the thickness of the base film may be 25 μm or more and 150 μm or less, preferably 38 μm or more and 130 μm or less, and more preferably 50 μm or more and 125 μm or less.

[0092] The substrate film here may be a transparent substrate film, and being transparent means that the light transmittance of visible light (400 to 700 nm) is 80% or more.

[0093] When the base film has the above range, the laminated protective film has the property of being thinnable, and has the characteristic of being able to sufficiently protect the adherend from external impact when applied to subsequent processes.

[0094] In one embodiment of the present application, the thickness of the pressure-sensitive adhesive film may be 10 μm or more and 100 μm or less.

[0095] In another embodiment, the thickness of the pressure-sensitive adhesive film may be 10 μm or more and 100 μm or less, preferably 12 μm or more and 75 μm or less, and more preferably 15 μm or more and 50 μm or less.

[0096] When the thickness of the adhesive film is within the above range, the rate of air bubbles generated inside the adhesive film is low, and as a result, when adhered to an adherend, the adhesive film has the characteristics of excellent adhesive strength, no lifting phenomenon, and no dent problem.

[0097] In one embodiment of the present application, the surface of the base film that contacts the adhesive film may include an antistatic layer. In this case, the surface of the base film opposite to the surface of the adhesive film that contacts the adhesive film may include the antistatic hard coating layer.

[0098] According to one embodiment of the present invention, the pressure-sensitive adhesive film is provided on one side of an antistatic layer, thereby reducing the amount of accumulated static electricity. In addition, since the surface resistance of the pressure-sensitive adhesive film is reduced, the generation of static electricity on the surface of the pressure-sensitive adhesive film can be reduced when the protective layer is peeled off from the surface protective film.

[0099] Therefore, when the protective layer is removed from the surface protective film in order to attach the adhesive film to the surface of the adherend, or when the surface protective film is peeled off from the surface of the adherend, it is possible to prevent foreign matter that may be attached to the adhesive film or the adherend due to static electricity, and it is also possible to prevent contamination of the adherend surface during the process and prevent deterioration of the properties of the adherend surface.

[0100] In this specification, the term "antistatic layer" means a layer intended to suppress the generation of static electricity.

[0101] The antistatic layer may be formed by a known method to achieve the desired effect. For example, the antistatic layer may be formed on one or both sides of the substrate layer by an in-line coating method.

[0102] In the present invention, the antistatic layer may be made of an appropriate antistatic composition in consideration of the object of the present application. For example, the first antistatic layer may include, but is not limited to, one selected from the group consisting of an acrylic resin, a urethane resin, a urethane-acrylic copolymer, an ester resin, an ether resin, an amide resin, an epoxy resin, and a melamine resin, or a mixture thereof.

[0103] In one embodiment, the antistatic layer may include a conductive material, which may include, but is not limited to, a conductive polymer or a carbon nanotube.

[0104] The conductive polymer may include, for example, polyaniline, polypyrrole, polythiophene, derivatives or copolymers thereof, but is not limited thereto.

[0105] The carbon nanotube may have a tube shape formed by rolling up a graphite plate formed of hexagonal rings each having six carbon atoms. The carbon nanotube has excellent rigidity and electrical conductivity, and when used as an antistatic layer of a surface protective film, the hardness of the antistatic layer is increased, and the antistatic function is improved.

[0106] The thickness of the antistatic layer may be appropriately selected in consideration of the object of the present application, and may be 10 nm or more; or 20 nm or more. In one embodiment, the thickness of the antistatic layer may be 400 nm or less; 300 nm or less; or 100 nm or less. When the thickness of the antistatic layer satisfies the range of 10 nm or more and 400 nm or less, the base film can have excellent coating properties.

[0107] In one embodiment, the surface resistance of the antistatic layer may be appropriately selected in consideration of the object of the present application. For example, the surface resistance of the first antistatic layer is independently 10 4 Ω / sq or more;10 5 Ω / sq or more;10 6 Ω / sq or more;10 7 Ω / sq or more;10 8 Ω / sq or more; or 10 9 For example, the surface resistance of the antistatic layer is independently 5×10 12 Ω / sq or less; or 10 11 When the antistatic layer has a surface resistance within the above range, the surface protective film can have an excellent antistatic function.

[0108] In one embodiment of the present application, there is provided a surface protective film, wherein the thickness of the surface protective film is 35 μm or more and 250 μm or less.

[0109] In another embodiment, the thickness of the surface protective film may be 35 μm or more and 250 μm or less, preferably 50 μm or more and 200 μm or less, and more preferably 60 μm or more and 150 μm or less.

[0110] By having the surface protection film fall within the above range, the film has the characteristics of having an appropriate thickness when subsequently applied to an adherend, not causing a decrease in adhesive strength, and being able to provide a surface protection film with excellent reliability even after repeated folding / unfolding several times.

[0111] In one embodiment of the present application, the pressure-sensitive adhesive film may be laminated in multiple layers. In one embodiment of the present application, there is provided a surface protection film further comprising a release sheet on the surface of the pressure-sensitive adhesive film opposite to the surface in contact with the base film.

[0112] The phrase "including a release sheet on one surface of the adhesive film" means that a release sheet is provided on the surface of the adhesive film opposite to the surface in contact with the base film.

[0113] In one embodiment of the present application, the release sheet may be a hydrophobic film, which refers to a transparent layer attached to one side of an adhesive film as a layer for protecting a very thin adhesive sheet, and may be a film having excellent mechanical strength, thermal stability, moisture shielding properties, isotropy, etc. For example, acetate-based films such as triacetyl cellulose (TAC), polyester-based films, polyethersulfone-based films, polycarbonate-based films, polyamide-based films, polyimide-based films, polyolefin-based films, cycloolefin-based films, polyurethane-based films, and acrylic-based films may be used, but are not limited to these as long as they are commercially available silicone-treated release sheets. The release sheet may be removed entirely upon application as a surface protection material for processing.

[0114] One embodiment of the present application provides a method for producing a surface protection film, comprising the steps of: preparing a polyurethane-based pressure-sensitive adhesive composition according to the present application; adding a curing agent to the polyurethane-based pressure-sensitive adhesive composition; and coating the polyurethane-based pressure-sensitive adhesive composition onto a substrate film.

[0115] In the method for producing a surface protective film, the polyurethane-based pressure-sensitive adhesive composition is as described above.

[0116] In one embodiment of the present application, there is provided a method for producing a surface protection film, comprising the steps of: coating the polyurethane-based pressure-sensitive adhesive composition on a substrate film; drying the polyurethane-based pressure-sensitive adhesive composition; and thermally curing the polyurethane-based pressure-sensitive adhesive composition.

[0117] One embodiment of the present disclosure provides a method for manufacturing an organic light emitting electronic device. In one embodiment of the present specification, the method for manufacturing the organic light-emitting electronic device includes attaching the adhesive film of the surface protection film onto the encapsulation layer of the organic light-emitting element.

[0118] That is, the present invention provides a method for manufacturing an organic light-emitting electronic device, comprising the steps of: attaching a surface protection film including a substrate film; and an adhesive film including the polyurethane-based adhesive composition of the present application or a cured product thereof provided on one side of the substrate film, onto an encapsulating layer of an organic light-emitting element.

[0119] In one embodiment, when the surface protective film further includes a protective layer, the method for manufacturing the organic light-emitting electronic device further includes a step of removing the protective layer from the surface protective film before the step of adhering the adhesive layer onto the sealing layer.

[0120] In one embodiment of the present specification, the organic light emitting device includes, in order, a glass, a plastic substrate, a thin film transistor, an organic light emitting diode, and an encapsulation layer.

[0121] 2 is a diagram illustrating an example of a state in which a surface protection film according to an embodiment of the present invention is attached onto an encapsulation layer during a manufacturing process of an organic light emitting electronic device. Referring to Fig. 2, the surface protection film of Fig. 1 according to an embodiment of the present invention is attached onto an encapsulation layer 515 of an organic light emitting device 510 including glass 511, a plastic substrate 512, a thin film transistor 513, an organic light emitting diode 514, and an encapsulation layer 515 in that order, such that the adhesive film 20 and the encapsulation layer 515 face each other.

[0122] The encapsulation layer may exhibit excellent moisture blocking properties and optical properties in an organic light emitting electronic device, and may be formed as a stable encapsulation layer regardless of the shape of the organic light emitting electronic device, such as top emission or bottom emission.

[0123] In one embodiment, the sealing layer may include a single or multiple inorganic layers. The sealing layer may be formed by a method known in the art.

[0124] The single or multi-layer inorganic layer may include, for example, an aluminum oxide-based material, a silicon nitride-based material, a silicon oxynitride-based material, or the like.

[0125] The method for manufacturing an organic light-emitting electronic device of the present application may further include the steps of peeling the surface protection film from the encapsulation layer; and laminating a touch screen panel and a cover window on the encapsulation layer. The surface protection film exhibits excellent antistatic properties to the encapsulation layer when peeled from the encapsulation layer, and therefore, when a touch screen panel is bonded onto the encapsulation layer, foreign matter can be prevented from adhering between the encapsulation layer and the touch screen, thereby preventing device defects. EXAMPLES

[0126] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the preferred embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in various different forms and should not be construed as being limited to the preferred embodiments set forth herein.

[0127] <Production Example> <Manufacture of surface protection film> Preparation Example 1: Preparation of adhesive composition Into a 2 L five-neck reactor, 10 parts of a bifunctional ether polyol (PPG with 20% EO added, product name: SC2204 from KPX Corporation) and 90 parts of a trifunctional ether polyol (product name: SC3314 from KPX Corporation) were added per 100 parts by weight of polyol, followed by the addition of an isocyanate, H12MDI (Evonik Corporation), in an amount such that the OH / NCO (molar ratio of functional groups) was 1.5, and then 40 parts by weight of toluene were added (non-volatile content 71%). While the temperature was raised from room temperature (25° C.) to 80° C. and maintained at that temperature, the disappearance of the remaining isocyanate groups was confirmed by IR spectroscopy, the reaction was terminated, and the resin was discharged.

[0128] Preparation Example 2: Preparation of adhesive composition It was produced in the same manner as in Production Example 1, except that 20 parts of bifunctional ether polyol (PPG) and 80 parts of trifunctional ether polyol (PPG) were added (non-volatile content 71%).

[0129] Production Example 3 - Production of adhesive composition It was produced in the same manner as in Production Example 1, except that 20 parts of bifunctional ether polyol (PPG + EO) and 80 parts of trifunctional ether polyol (PPG) were added (non-volatile content 71%).

[0130] Production Example 4 - Production of adhesive composition It was produced in the same manner as in Production Example 3, except that the amount of isocyanate H12MDI was changed to such an amount that the OH / NCO ratio was 1.45 (non-volatile content 71%).

[0131] Preparation Example 5 - Preparation of adhesive composition It was produced in the same manner as in Production Example 1, except that 20 parts of bifunctional ether polyol (PPG) and 80 parts of trifunctional ether polyol (PPG + EO) were added (non-volatile content 71%).

[0132] Preparation Example 6 - Preparation of adhesive composition It was produced in the same manner as in Production Example 1, except that 30 parts of bifunctional ether polyol (PPG) and 70 parts of trifunctional ether polyol (PPG + EO) were added (non-volatile content 71%).

[0133] Preparation Example 7 - Preparation of adhesive composition The same production method as in Production Example 1 was used to produce a polyether polyol (PPG+EO) of 20 parts, a polyether polyol (PPG) of 80 parts, and a polyether polyol (PPG) of 30 parts. The amount of isocyanate H12MDI was changed to an amount such that the OH / NCO ratio was 1.6 (non-volatile content 71%).

[0134] Preparation Example 8 - Preparation of adhesive composition It was produced in the same manner as in Production Example 7, except that the amount of isocyanate H12MDI was changed to such an amount that the OH / NCO ratio was 1.65 (non-volatile content 71%).

[0135] Comparative Preparation Example 1: Preparation of adhesive composition The same production method as in Production Example 1 was used to produce a copolymer, except that 70 parts of a bifunctional ether polyol (PPG) and 30 parts of a trifunctional ether polyol (PPG) were added and the OH / NCO ratio was adjusted to 1.2 (non-volatile content 71%).

[0136] Comparative Preparation Example 2: Preparation of adhesive composition It was produced in the same manner as in Comparative Production Example 1, except that 80 parts of bifunctional ether polyol (PPG) and 20 parts of trifunctional ether polyol (PPG) were added (non-volatile content 71%).

[0137] Comparative Preparation Example 3: Preparation of adhesive composition It was produced in the same manner as in Comparative Production Example 1, except that 90 parts of bifunctional ether polyol (PPG) and 10 parts of trifunctional ether polyol (PPG) were added (non-volatile content 71%).

[0138] Comparative Preparation Example 4 - Preparation of adhesive composition The same method as in Preparation Example 1 was used to produce the copolymer, except that 20 parts of a bifunctional ester polyol and 80 parts of a trifunctional ether polyol (PPG) were added (non-volatile content 71%).

[0139] Comparative Preparation Example 5 - Preparation of adhesive composition The same method as in Production Example 1 was used to produce the copolymer, except that 100 parts of bifunctional ether polyol (PPG+EO) was added and the OH / NCO ratio was adjusted to 1.1 (non-volatile content 71%).

[0140] Comparative Preparation Example 6 - Preparation of adhesive composition The same production method as in Production Example 1 was used to produce a copolymer (non-volatile content 71%), except that 100 parts of bifunctional ether polyol (PPG+EO) was added.

[0141] Comparative Preparation Example 7 - Preparation of adhesive composition A copolymer was produced in the same manner as in Comparative Production Example 5, except that the OH / NCO ratio was adjusted to 1.3 (non-volatile content 71%).

[0142] Comparative Preparation Example 8 - Preparation of adhesive composition The same production method as in Production Example 3 was used to produce a copolymer (non-volatile content 71%), except that the OH / NCO ratio was adjusted to 1.2.

[0143] Comparative Preparation Example 9 - Preparation of adhesive composition The same preparation as in Preparation Example 1 was carried out, except that 100 parts by weight of toluene was added (non-volatile content: 50%). 15 parts by weight of a polyfunctional isocyanate curing agent was added to 100 parts by weight of each of Preparations 1 to 8 and Comparative Preparations 1 to 9 based on the solid content, and the mixture was thoroughly stirred, coated on a polyester (PET) film, and dried in an oven at 140° C. for 3 minutes to prepare a polyurethane adhesive layer with a thickness of 75 μm. Then, the mixture was aged in an oven at 50° C. for 120 hours.

[0144] In producing the adhesive layer as described above, in the case of Comparative Preparation Example 6, coating was not performed due to gelation during the resin production process, and the adhesive compositions of Comparative Preparation Examples 7 and 8 were outside the viscosity range of the composition itself, and coating did not proceed due to poor coatability. The OH / NCO functional group ratio, molecular weight, viscosity, polyol composition and content for Production Examples 1 to 8 and Comparative Production Examples 1 to 9 are shown in Table 1 below.

[0145] [Table 1]

[0146] The low-speed and high-speed peel strengths of the adhesive layers according to Preparation Examples 1 to 8 and Comparative Preparation Examples 1 to 9 are shown in Table 2. Furthermore, in the case of Comparative Preparation Example 6, coating was not performed due to gelation during the resin production process, and the adhesive compositions of Comparative Preparation Examples 7, 8, and 9 were outside the viscosity range of the composition itself, and coating did not proceed due to poor coatability, so the high-speed and low-speed peel strengths themselves could not be measured.

[0147] [Table 2]

[0148] As can be seen from Tables 1 and 2, in the case of the polyurethane-based pressure-sensitive adhesive compositions of Examples 1 to 8, the contents of the bifunctional polyol and trifunctional polyol satisfy a specific range, and it has been found that the hydroxyl groups of the urethane polyol can be controlled to effectively adjust the urethane crosslink density.

[0149] In addition, it was confirmed that the adhesive composition had a viscosity within a specific range, which resulted in small thickness deviation relative to the substrate during adhesive coating and excellent coating properties. In particular, it was confirmed that the adhesive compositions of Comparative Preparation Examples 7 to 9 were outside the viscosity range and had poor coatability, resulting in no coating.

[0150] It was confirmed that the polyurethane-based pressure-sensitive adhesive compositions of Examples 1 to 8 were able to reduce removability at high speeds and minimize damage to the adherend when peeled off after being attached to the adherend. [Explanation of symbols]

[0151] 10. Base film 20 ···Adhesive film 40 Surface protection film 510 Organic light-emitting device 511 Glass 512 Plastic Substrate 513 Thin film transistor 514 Organic Light Emitting Diode 515 Sealing layer

Claims

1. A polyurethane polymer comprising a difunctional polyol and a trifunctional polyol; and A polyurethane-based pressure-sensitive adhesive composition containing an isocyanate-based crosslinking agent, The pressure-sensitive adhesive composition has a viscosity of 1,000 cPs (1 Pa s) or more and 10,000 cPs (10 Pa s) or less under conditions of 25° C. and 60% relative humidity, 5 to 40 parts by weight of a bifunctional polyol per 100 parts by weight of the total of the bifunctional polyol and the trifunctional polyol, and The trifunctional polyol is contained in an amount of 60 to 95 parts by weight per 100 parts by weight of the total of the bifunctional polyol and the trifunctional polyol, The polyurethane-based pressure-sensitive adhesive composition has a glass transition temperature of −50° C. or more and 0° C. or less, The polyurethane-based pressure-sensitive adhesive composition, wherein the bifunctional polyol and the trifunctional polyol are ether polyols.

2. The polyurethane polymer comprises a solvent, the solvent comprising The polyurethane-based pressure-sensitive adhesive composition according to claim 1 , wherein the polyol is contained in an amount of 5 parts by weight or more and 35 parts by weight or less relative to 100 parts by weight of the total of the bifunctional polyol and the trifunctional polyol.

3. 2. The polyurethane-based pressure-sensitive adhesive composition according to claim 1, wherein the molar ratio (-OH / NCO) of hydroxyl groups to isocyanate functional groups of the polyurethane polymer is 1.3 or more and 1.7 or less.

4. The polyurethane-based pressure-sensitive adhesive composition according to claim 1 , wherein the polyurethane polymer has a molecular weight of 50,000 g / mol or more and 200,000 g / mol or less.

5. The polyurethane-based pressure-sensitive adhesive composition according to claim 1, further comprising at least one selected from the group consisting of a solvent, a curing agent, a dispersing agent, a photoinitiator, a thermal initiator, a silane coupling agent, a plasticizer, a tackifier, and an antistatic agent.

6. A substrate film; and An adhesive film comprising the polyurethane-based adhesive composition according to any one of claims 1 to 5 or a cured product thereof provided on one surface of the base film; A surface protection film comprising:

7. The surface protective film according to claim 6, wherein when one side of the adhesive film is bonded to a glass substrate and then peeled off at a peel angle of 180° and a speed of 1.8 m / min, the low-speed peel force is 5 gf / inch (19.3 x 1.0 N / cm) or more, and when one side of the adhesive film is bonded to a glass substrate and then peeled off at a peel angle of 180° and a speed of 20 m / min, the high-speed peel force is 50 gf / inch (193 x 1.0 N / cm) or less.

8. The surface protective film according to claim 6 , wherein the thickness of the base film is 25 μm or more and 150 μm or less.

9. The surface protective film according to claim 6 , wherein the adhesive film has a thickness of 10 μm or more and 100 μm or less.

10. The surface protective film according to claim 6 , further comprising a release sheet on a surface of the pressure-sensitive adhesive film opposite to the surface in contact with the base film.

11. 7. The surface protective film according to claim 6, wherein the base film is selected from the group consisting of polyethylene terephthalate (PET), polycarbonate (PC), polyimide (PI), polyethylene naphthalate (PEN), polyethylene ether ketone (PEEK), polyarylate (PAR), polycylicolefin (PCO), polynorbornene, polyethylene (PES), and cycloolefin polymer (COP).

12. A step of preparing the polyurethane-based pressure-sensitive adhesive composition according to any one of claims 1 to 5; adding a curing agent to the polyurethane-based pressure-sensitive adhesive composition; and coating the polyurethane-based pressure-sensitive adhesive composition onto a substrate film; A method for producing a surface protection film comprising the steps of:

13. After the step of coating the polyurethane-based pressure-sensitive adhesive composition on a substrate film, drying the polyurethane-based pressure-sensitive adhesive composition; and a step of thermally curing the polyurethane-based pressure-sensitive adhesive composition; The method for producing a surface protective film according to claim 12, comprising:

14. A method for manufacturing an organic light-emitting electronic device, comprising: a substrate film; and an adhesive film comprising the polyurethane-based adhesive composition according to any one of claims 1 to 5 or a cured product thereof provided on one side of the substrate film, the adhesive film being attached to an encapsulating layer of an organic light-emitting element.

15. The method of claim 14 , wherein the organic light emitting device comprises, in order, a glass, a plastic substrate, a thin film transistor, an organic light emitting diode, and an encapsulation layer.

16. 15. The method for manufacturing an organic light-emitting electronic device according to claim 14, further comprising the steps of: peeling the surface protection film from the encapsulation layer; and laminating a touch screen panel and a cover window on the encapsulation layer.

Citation Information

Patent Citations

  • Adhesive-backed article

    JP2006299283A

  • Removable adhesive

    JP2016186062A

  • Pressure-sensitive adhesive and film and laminate using the same

    JP2017137396A

  • Pressure-sensitive adhesive, and adhesive film

    JP2018062628A