Medical hydrogels containing nanofibrillated cellulose, individualized wound dressings, and methods for preparing the same

Nanofibrillar cellulose hydrogels address the challenges of deep wound healing by inducing angiogenesis and reducing scarring, offering a moldable, non-sticky solution for deep wounds that enhances vascularization and healing efficacy.

JP7567145B2Active Publication Date: 2024-10-16UPM KYMMENE OYJ
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020128682
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-29
Filing Date
2020-07-29
Publication Date
2024-10-16
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Deep wounds, particularly those affecting the dermis and underlying tissues, are difficult to treat due to challenges such as incomplete healing, severe scarring, and susceptibility to bacterial infections, with existing dressings often sticking to the wound and failing to promote adequate healing.

Method used

The development of medical hydrogels containing nanofibrillar cellulose, specifically anionically modified to a diameter of 200 nm or less, with a concentration of 1 to 3.5% (w/w), which are moldable, non-sticky, and promote angiogenesis by activating fibroblasts, providing a moist environment for wound healing.

Benefits of technology

The nanofibrillar cellulose hydrogels effectively induce vascularization, reduce scarring, and enhance wound healing by maintaining contact with deep tissues without damage, while being easily removable and promoting a favorable healing environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567145000002
    Figure 0007567145000002
  • Figure 0007567145000003
    Figure 0007567145000003
  • Figure 0007567145000004
    Figure 0007567145000004
Patent Text Reader

Abstract

To provide a medical hydrogel for use for inducing vascularization in wounds and / or for treating deep wounds of dermis and / or below tissue.SOLUTION: There is provided a medical hydrogel comprising nanofibrillar cellulose, wherein the content of nanofibrillar cellulose in the hydrogel is in the range of 1 to 3.5% (w / w), and the nanofibrillar cellulose comprises anionic nanofibrillar cellulose having an average fibril diameter of 200 nm or less, and is also provided a preparation method thereof.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a medical hydrogel comprising nanofibril cellulose and a method for preparing the same, more particularly to a medical hydrogel comprising nanofibril cellulose for treating wounds, in particular for inducing angiogenesis in said wounds, and also to a medical hydrogel used for inducing angiogenesis in wounds and / or for treating deep wounds in the dermis and / or in the tissues below. [Background technology]

[0002] Wounds, especially deep wounds, can be difficult to treat. In particular, wounds that involve damage to the dermis or even deeper tissues can be difficult to heal and can result in severe scarring. In many cases, the patient's body grows scar tissue very quickly, resulting in the deep wound never healing completely. Instead, only the surface of the wound heals, but the lining is not yet fully formed. Deeper wounds, which in some cases are dirtier and larger, are more susceptible to bacterial infection. As a result, this slows down the entire healing process.

[0003] Dressings may be applied to wounds. However, dressings may stick to the wound and may not encourage the healing of deep wounds properly. There is a need to improve the treatment of wounds, especially deep wounds, and to find better materials and methods for this treatment. In particular, it is desirable to improve the healing of deep tissues. These materials should be moldable to deep wounds and removable so that the wound is not further damaged but the healing of the deep wound is initiated and maintained. Summary of the Invention [Problem to be solved by the invention]

[0004] It has been found that the healing of deep wounds (such as those involving the dermis and / or deeper tissues) can be improved by applying a specific type of nanofibrillar cellulose hydrogel into and / or onto the wound. The hydrogel is capable of inducing angiogenesis or pre-vascularization in the deep tissues, which significantly accelerates the healing process in the wound. Also, the results are better, with less scarring, compared to when conventional materials are used to treat similar wounds. [Means for solving the problem]

[0005] The present application, Providing an anionically modified pulp; or providing a pulp and anionically modifying the pulp; The anion-modified pulp is treated until nanofibril cellulose with an average fibril diameter of 200 nm or less is obtained. Disintegration To do, If desired, Disintegration homogenizing the anionically modified pulp in one or more non-fibrillating homogenization steps; and The nanofibril cellulose is made into a medical hydrogel having a nanofibril cellulose content in the range of 1 to 3.5% (w / w); The present invention provides a method for preparing a medical hydrogel, comprising:

[0006] The present application also provides a medical hydrogel containing nanofibril cellulose, in which the content of nanofibril cellulose in the hydrogel is within the range of 1 to 3.5% (w / w), and the nanofibril cellulose includes anionic nanofibril cellulose having an average fibril diameter of 200 nm or less.

[0007] The present application also provides a medical hydrogel comprising nanofibril cellulose for use in inducing angiogenesis in wounds.The present application also provides a medical hydrogel comprising nanofibril cellulose for treating deep wounds in the dermis and / or under tissue, preferably for use in inducing angiogenesis.

[0008] The present application, providing a medical hydrogel as disclosed herein; Obtaining a digital three-dimensional model of an object designed to fit a wound; and preparing a three-dimensional object from said medical hydrogel according to said digital three-dimensional model by additive manufacturing to obtain a wound dressing tailored to fit said wound, The present invention provides a method for preparing a tailored wound dressing, comprising:

[0009] The present application also provides a wound dressing tailored to fit a wound, the wound dressing comprising a medical hydrogel as disclosed herein, the wound dressing being tailored to fit the wound, the wound dressing may be obtained by an additive manufacturing process as disclosed herein.

[0010] The present application also discloses kits containing the medical hydrogels described above packaged in one or more sealed packages or in one or more application devices, such as syringes, applicators, pumps or tubes.

[0011] Main embodiments are characterized in the independent claims. Various embodiments are disclosed in the dependent claims. The embodiments and examples recited in the claims and in the description are freely combinable with one another, unless expressly stated otherwise.

[0012] It has been found that hydrogels comprising nanofibrillar cellulose and having certain physical properties in certain ranges (particularly relatively low viscosity and consistency) are particularly suitable for medical purposes (particularly as medical products such as moldable products that can be used as dressings, etc.). When applied to a wound, the hydrogel exhibited properties such as solidity, low adhesion, sufficient fracture toughness expressed as compression work, formability, and good removability or detachability. It is important that the material does not stick to the wound, especially deep tissue, so that when the hydrogel is removed, it does not damage the tissue or break into the wound. It is also important that the hydrogel remains in the wound during use and maintains adequate contact with the tissue. These properties were obtained with the material. Moreover, the material promoted the healing of especially deep wounds or other damage or injuries to such tissue.

[0013] The hydrogels disclosed herein provide good water retention capacity and molecular diffusivity rates, properties that are desirable in medical applications such as wound treatment.

[0014] The hydrogels described herein are useful in medical applications where the material is in contact with living tissue. It has been discovered that nanofibril cellulose exhibits unique properties when applied to damaged areas, especially when the damage is in deep tissues such as the dermis, adipose tissue, or other deep tissues. The products containing nanofibril cellulose described herein are highly biocompatible with living tissues and provide several beneficial effects. Without being bound to any particular theory, it is believed that hydrogels containing highly hydrophilic nanofibril cellulose, which has a very high specific surface area and therefore high water retention, when applied to tissue, provide a good moist environment between the tissue or wound and the nanofibril cellulose. The large amount of free hydroxyl groups in the nanofibril cellulose allows hydrogen bonds to form between the nanofibril cellulose and water molecules, allowing gel formation and high water retention of the nanofibril cellulose. The nanofibrillar cellulose hydrogel contains a large amount of water, which is presumably the main source of contact with tissue, and allows for the transfer of fluids and / or drugs from the wound to the hydrogel or from the hydrogel to the wound.The products disclosed herein have a relatively low viscosity and consistency, which surprisingly enhances these effects and provides additional new effects.

[0015] One particular effect found when using the hydrogels described herein was that angiogenesis was induced in the damaged area. This is particularly advantageous when proper healing of the damaged area in deep wounds is desired. Without proper angiogenesis, the damaged area will be heavily scarred, resulting in incomplete healing. More specifically, the anionic nanofibril cellulose gel activated fibroblasts in the skin and then induced the formation of blood vessels, i.e., angiogenesis, in the damaged area. This effect was higher compared to the angiogenesis obtained by a chemically unmodified nanofibril cellulose gel with similar properties.

[0016] When hydrogels are used to cover wounds or other injuries or damage, they also provide other benefits: The product has good utility because it can be easily applied and removed without damage (e.g., disintegration). The product maintained its shape. The hydrogel protects the wound from infection and provides a moist environment for the wound to heal. The hydrogel does not adhere to the damaged skin, tissue, or wound in an irreversible manner as do conventional materials, which are usually very difficult to remove without damaging the healed or to-be-healed area. The condition between the product and the skin encourages healing of the damaged area.

[0017] Hydrogels may be used to controllably and effectively deliver or impart agents (e.g., therapeutic agents) to a subject (e.g., a patient or user) by, for example, a transdermal route or by other routes. Controlled release refers, for example, to obtaining a desired release rate and / or profile of the agent(s) over a period of time, and may be influenced by the choice of gel, for example, the gel percentage or gel thickness, the concentration or form of the releasable agent(s), the presence of any auxiliary agents, or other conditions such as pH, temperature, etc. that affect the release rate and / or activity of the releasable agent. The combined effect of the special conditions and release characteristics between the tissue and the hydrogel as described above provides an efficient delivery of the substance into the living tissue. Meanwhile, the hydrogel may also absorb substances (e.g., wound exudate) from the wound or damaged area. This may also promote healing. Nanofibrillar cellulose hydrogels provide a hydrophilic matrix that is non-toxic, biocompatible, and also biodegradable. For example, the matrix may be enzymatically degraded. On the other hand, hydrogels are stable under physiological conditions. [Brief description of the drawings]

[0018] [Figure 1A] Figure 1 shows histopathological evaluation of wounds in humanized mice treated with NFC dressings (type 1 dressings).Figure 1A shows an untreated injury. [Figure 1B]1A-1D show histopathological evaluation of wounds in humanized mice treated with NFC dressings (Type 1 dressings). FIG. 1B shows a wound treated with Type 1 dressing. [Figure 2A] Figure 2 shows wound dressing studies with 3.2% anionic nanofibril cellulose (ANFC) hydrogel, unmodified nanofibril cellulose and control samples (no treatment). Figure 2A shows a photograph of a wound surrounded by a silicone ring sutured onto the surface of the skin that encloses the wound and prevents contraction, and wound dressings are applied within the ring (except for the control). [Figure 2B] Figure 2B shows a wound dressing study with 3.2% anionic nanofibril cellulose (ANFC) hydrogel, unmodified nanofibril cellulose, and a control sample (no treatment). Figure 2B shows a graph comparing the percentage of wound closure at days 3 and 7. [Figure 3A] Results from stimulation of fibroblast activation are shown in Figure 3. Figure 3A shows α-SMA staining to detect vascular networks and fibroblast activation in histological skin samples. [Figure 3B] Figure 3B shows the results from the stimulation of fibroblast activation. Figure 3B shows a graph presenting the α-SMA staining intensity in the different samples. [Figure 4A] Figure 4 shows a chicken study of 3.27% NFC hydrogel. Figure 4A shows the hydrogel in the wound. [Figure 4B] Figure 4B shows a chicken study of 3.27% NFC hydrogel. Figure 4B shows the hydrogel removed from the wound. [Figure 5A] Figure 5 shows a chicken study of 2.65% NFC hydrogel. Figure 5A shows the hydrogel in the wound. [Figure 5B] Figure 5B shows a chicken study of 2.65% NFC hydrogel. Figure 5B shows the hydrogel removed from the wound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In this specification, percentage values ​​are on a weight basis (w / w) unless otherwise indicated. When any numerical range is given, the range is inclusive of the upper and lower limits. The open term "comprising" also includes as an alternative the closed term "consisting of."

[0020] The materials and products described herein may be medical and / or scientific materials and products, such as life science materials and products, and may be used in methods and applications involving living tissue and / or bioactive materials or substances, such as those described herein. The materials or products may be or relate to medical treatment materials or products, may be used in methods involving wounds, injuries and other damage to tissues, such as the skin or tissue(s) below the skin, and / or may be used for medical or scientific purposes or in other related applicable methods. In particular, the materials and products are applied to wounds, such as wounds involving the dermis and / or deeper tissue(s), i.e. wounds including damage in the tissue(s) where such treatment is particularly desired, and in particular for application to deep wounds. Not all medical products, even in hydrogel form, are applicable to wounds, especially deep wounds, which require products with properties that do not damage or irritate deep tissues, nor are they capable of being simultaneously molded to fit within the wound, nor are they capable of being removed from the wound, preferably without damaging and destroying the wound.

[0021] The term "medical" is used for products or uses where the product (i.e., a product comprising the hydrogel of the embodiment) is used or suitable for medical purposes. Medical products are sterile or sterilizable, i.e., the product is resistant to sterilization processes, for example, by using temperature, pressure, moisture, chemicals, radiation, or a combination thereof. The product may be, for example, autoclaved or other methods using high temperatures may be used. In one example, the product is autoclaved at 121°C for 15 minutes. It may also be desirable for medical products to be pyrogen-free and free of undesirable protein residues, undesirable bioactive materials, animal-derived materials, etc. In particular, for anionic nanofibrillar cellulose, UV or gamma radiation sterilization may be used.

[0022] Nanofibrillar cellulose (NFC) hydrogels (such as anionic NFC hydrogels) may also be capable of sustained or controllable release and / or retention of active agents, such as therapeutic agents (e.g. pharmaceutical ingredients), or other bioactive agents, as a function of time, particularly at constant temperature and pH. The hydrogel may also include one or more antibacterial or antimicrobial agent(s) and / or other therapeutic agent(s) that may promote wound healing. The content of the agent(s) in the hydrogel may be in the range of 0.01-1% (w / w), such as 0.05-0.5% (w / w), or another suitable physiologically effective amount.

[0023] The nanofibrillary cellulose may have a suitable degree of fibrillation, which may be characterized, for example, by the rheological properties of the material and / or the diameter of the fibrils or fibril bundles. For example, the nanofibrillary cellulose, when dispersed in water, may have a zero shear viscosity in the range of 1000-100000 Pa·s, preferably 1000-50000 Pa·s (such as 2000-20000 Pa·s) for anionic grades, and a yield stress in the range of 1-50 Pa, preferably 1-30 Pa (such as 3-15 Pa), measured by a rotational rheometer at a consistency of 0.5% by weight (w / w) in an aqueous medium at 22° C.±1° C.

[0024] It was found that the hydrogel for treating deep wounds and promoting angiogenesis in the wounds preferably has a specific viscosity required for the concentration of the hydrogel. The preferred viscosity is significantly lower than the related prior art products, and surprisingly, such hydrogels can activate fibroblasts in deep tissues and efficiently induce angiogenesis in deep wounds. The hydrogels with the above viscosity at the concentrations used remain well in the deep wounds without causing damage or irritation to the deep tissues, and are also easy to remove from the wounds. The hydrogels maintain their activity, such as angiogenic effects, for several days. After this treatment period, the wounds are healed and in a stable state, such that they can be further treated and / or covered with other products, such as drugs and / or other NFC hydrogels or NFC-containing products (e.g., gauze, etc.), or can be surgically treated.

[0025] In one embodiment, there is provided a medical hydrogel comprising nanofibril cellulose, the hydrogel having a viscosity measured by a viscometer at 37°C at a shear rate of 0.1 (1 / sec) at the concentration of the hydrogel being within the range of 500 to 2200 Pa·s (e.g., 500 to 2000 Pa·s, 500 to 1800 Pa·s, 700 to 2000 Pa·s, or 1000 to 2000 Pa·s, etc.). In one embodiment, the hydrogel has a viscosity measured by a viscometer at 37°C at a shear rate of 0.1 (1 / sec) at the concentration of the hydrogel being within the range of 700 to 1800 Pa·s (e.g., 1000 to 1800 Pa·s, etc.). In one embodiment corresponding to certain advantageous tested hydrogels, the viscosity measured by a viscometer at 37° C. at a shear rate of 0.1 (1 / sec) at the concentration of the hydrogel is in the range of 1500-2000 Pa·s. These viscosities are measured at the concentration of the hydrogel as provided (i.e., “own concentration”) and may be in the range of 1-3.5% (w / w) as described herein, or in a narrower range. The viscosity at the own concentration may be measured by any suitable viscometer. In the tests, the viscosity was measured by a HAAKE Viscotester iQ Rheometer (Thermo Fisher Scientific, Karlsruhe, Germany) equipped with a Peltier system for temperature control. The above viscosity may be referred to as shear viscosity.

[0026] In order to control the properties of the hydrogel, especially when used as a wound dressing in deep wounds or in further manufacturing steps, it is necessary to make the nanofibrillary cellulose in the hydrogel a certain consistency (dry content), as disclosed herein. The hydrogel usually contains mainly or only an aqueous liquid, which may be, for example, water or an aqueous buffer solution and / or a saline solution. The hydrogel may be formed in the form of a physiological salt solution and therefore may contain salt, such as, for example, 0.8 to 1.0% (w / w) salt, for example, the salt includes sodium chloride.

[0027] The present application provides a medical hydrogel comprising nanofibril cellulose, the content of nanofibril cellulose in the hydrogel being within the range of 1-3.5% (w / w), and the nanofibril cellulose comprising anionic nanofibril cellulose having an average fibril diameter of 200 nm or less. The medical hydrogel may be moldable (particularly hand moldable), which makes it easy to mold the material to practically fit any type of wound. The nanofibril cellulose may be only anionic nanofibril cellulose, whereby no other type of nanofibril cellulose is present. The nanofibril cellulose may be the only fibrillar, fibrous, polymeric and / or organic material in the medical hydrogel, whereby in such a case no other matrix and / or reinforcing material may be present in addition to the nanofibril cellulose. Medical hydrogels preferably do not contain other reinforcing and / or matrix-like materials or structures (e.g. synthetic, semi-synthetic or natural polymers or other compounds such as collagen, proteins or peptides or other biopolymers, or plastic polymers).

[0028] The useful consistency of nanofibril cellulose is relatively narrow, ranging from 1 to 3.5% (w / w). At this consistency, the hydrogel contains a suitable amount of water, is well processable, and has suitable properties for the various medical applications disclosed herein, particularly the promotion of angiogenesis in deep wounds. The content of nanofibril cellulose in the hydrogel may be in the range of 1.1 to 3.5% (w / w). Depending on the wound type and dimensions, it may be desirable to use a hydrogel that does not disintegrate or otherwise break down easily. In such cases, the content of nanofibril cellulose in the hydrogel may be in the range of 1.1 to 3.3% (w / w) or 1.1 to 3.0% (w / w) (e.g., 1.5 to 3.5% (w / w), 1.5 to 3.3% (w / w), or 2.0 to 3.5% (w / w), etc.). However, on the other hand, lower concentrations may result in gels that may be sticky but flexible, and therefore may survive better in wounds or targets that are prone to movement. It has been found that when applying hydrogels to deep wounds, it is particularly important to use hydrogels with the above consistency or nanofibrillated cellulose content to avoid damage to sensitive deeper tissues and promote angiogenesis in said deep tissues. In tests, hydrogels with a consistency in the range of 2.0-3.5% (w / w) have been found to be advantageous for most applications, including manually molding and preparing preformed products. The healing properties for most deep wounds were also particularly good in the above range.

[0029] In some cases, it may be desirable to use a higher consistency of nanofibril cellulose, such as 2.0-3.5% (w / w), e.g., 2.5-3.5% (w / w), for example for 3D printing applications and / or to obtain a more moldable, tougher, less sticky and / or viscous hydrogel.

[0030] Some of the advantageous properties of hydrogels containing nanofibril cellulose include flexibility, elasticity and reshapeability. Hydrogels contain a lot of water, so they may also exhibit good diffusion and release properties of molecules. These properties are useful, for example, when hydrogels are used as coverings in healing wounds or in other medical applications, such as for delivery, storage and control of bioactive agents.

[0031] Flexibility is a desirable feature in many applications, such as medical applications. For example, flexible patches and dressings containing nanofibrillar cellulose hydrogels are useful for application on the skin, for example, to cover wounds and other damage or injuries, such as burns. A related desirable feature is moldability, especially if the hydrogel is to be applied to deep wounds. Viscosity generally correlates with this moldability. The viscosity must be high enough to maintain the structure of the composition, while being low enough to allow moldability and prevent cracking of the gel. Furthermore, having an optimal initial viscosity allows the viscosity of the pseudoplastic product to decrease during molding, making it easier to mold the gel into a desired shape.

[0032] A certain water retention capacity may be required to treat deep wounds and to promote angiogenesis in deep wounds. In one embodiment, a medical hydrogel is provided in which the water retention value of the nanofibril cellulose is in the range of 20-70 g water per 1 g dry hydrogel, preferably 23-50 g water per 1 g dry hydrogel (e.g., in the range of 25-35 g water per 1 g dry hydrogel, more specifically, less than 30 g water per 1 g dry hydrogel, e.g., 20-29 g water per 1 g dry hydrogel, or 25-29 g water per 1 g dry hydrogel). The water retention value can be measured by the ÅAGWR (Åbo Akademi Gravitometric Water Retention) method.

[0033] The present application, Providing an anionically modified pulp (such as wood pulp), - The pulp is processed until nanofibril cellulose having an average fibril diameter of 200 nm or less is obtained. Disintegration To do, -Optionally, Disintegration homogenizing the resulting pulp in one or more non-fibrillating homogenization steps; and - making the nanofibril cellulose into a medical hydrogel having a nanofibril cellulose content within the range of 1.1 to 3.5% (w / w) (e.g., 1 to 3.5% (w / w) (e.g., 2.0 to 3.5% (w / w))); The present invention provides a method for preparing a medical hydrogel, the method may include providing a pulp and anionically modifying the pulp, preferably to obtain a desired degree of modification (e.g., anionic charge, etc.).

[0034] The method may include converting the nanofibril cellulose into a medical hydrogel having a viscosity in the range of 500 to 2200 Pa·s (e.g., in the range of 700 to 1800 Pa·s) at a shear rate of 0.1 (1 / sec) at 37°C measured by a viscometer at a concentration of the hydrogel, or another viscosity disclosed herein.

[0035] The medical hydrogels described herein can be obtained by this method.

[0036] The medical hydrogel may be provided for use in inducing angiogenesis in wounds. More particularly, the medical hydrogel may be provided for use in treating deep wounds in the dermis and / or underlying tissue, preferably for inducing angiogenesis or thereby and / or activating fibroblasts. The medical hydrogel may be provided in a sealed packing or applicator, optionally packed in a kit. The packing or kit may include instructions for using the medical hydrogel for a particular purpose and / or in a particular method, such as those disclosed herein.

[0037] Healthy skin comprises three main components or layers: epidermis, dermis and subcutaneous tissue. The epidermis mainly contains keratinocytes and is mainly responsible for the barrier function of the skin, including preventing the entry of harmful pathogens into the body. From the outer to the inner layers, the epidermis comprises the stratum corneum, stratum lucidum, stratum granulosum, stratum spinosum and stratum basale. Beneath the stratum basale, a connecting layer known as the basement membrane region can be found between the epidermis and the dermis. The dermis contains fibroblasts and extracellular matrix components such as collagen and elastin, as well as blood vessels, nerves and accessory structures. The dermis contains two layers: the papillary dermis (upper layer), which is responsible for preventing sliding between the epidermis and dermis and for providing oxygen and nutrients to the epidermis, and the reticular dermis (lower layer), which is mainly responsible for the mechanical properties of the skin. The subcutaneous tissue, also called the subcutaneous tissue, contains mostly adipose tissue.

[0038] Nanofibril Cellulose The starting material for forming the above-mentioned medical hydrogel is nanofibril cellulose (also called nanocellulose), which refers to isolated cellulose fibrils or fibril bundles derived from cellulose raw materials. Nanofibril cellulose is based on a natural polymer that is abundant in nature. Nanofibril cellulose can form a viscous hydrogel in water. Nanofibril cellulose production technology involves the synthesis of fibrous raw materials. Disintegration (For example, by grinding an aqueous dispersion of pulp fibers to obtain nanofibrillated cellulose.) The nanofibrillated cellulose material obtained after such grinding or homogenization process is a thin viscoelastic hydrogel.

[0039] The resulting material is Disintegration Depending on the conditions, it is homogeneously dispersed in water and is usually present at a relatively low concentration. The starting material may be an aqueous gel at a concentration of 0.2-10% (w / w) (e.g., 0.2-5% (w / w)). Nanofibril cellulose is a fibrous raw material. Disintegration An example of a commercially available nanofibrillar cellulose hydrogel is GrowDex® by UPM.

[0040] Due to its nanoscale structure, nanofibril cellulose has unique properties that allow functionality that cannot be imparted by conventional cellulose. However, due to this nanoscale structure, nanofibril cellulose is also a challenging material. For example, it can be difficult to dehydrate or handle.

[0041] Nanofibril cellulose may be prepared from cellulose raw materials of plant origin or derived from certain bacterial fermentation processes. Nanofibril cellulose is preferably made from plant materials. The raw material may be based on any plant material containing cellulose. In one example, the fibrils are obtained from non-parenchymal plant materials. In such cases, these fibrils may be obtained from secondary cell walls. One of the abundant sources of such cellulose fibrils is wood fibers. Nanofibril cellulose may be produced by homogenizing fibrous raw materials derived from wood, which may be chemical pulp. Cellulose fibers are Disintegration The fibrils are then dehydrated to produce fibrils that are only a few nanometers in size (in most cases the average diameter can be 200 nm or less), resulting in fibrils dispersed in water. Fibrils originating from secondary cell walls are essentially crystalline with a crystallinity of at least 55%. Such fibrils may have different properties than fibrils originating from primary cell walls, for example dehydration of fibrils originating from secondary cell walls may be more challenging. Generally, in cellulose sources from primary cell walls such as sugar beet, potato tuber and banana rachis, microfibrils are more easily liberated from the fiber matrix than fibrils from wood, Disintegration However, these materials are still somewhat heterogeneous and consist of large fibril bundles.

[0042] Non-woody materials include those derived from agricultural residues, grasses, or other plant materials such as straw, leaves, bark, seeds, husks, flowers, rapeseed, or fruits from cotton, corn, wheat, oats, rye, barley, rice, linseed, hemp, abaca, sisal, jute, ramie, kenaf, bagasse, bamboo, or reeds. The cellulose raw material may be derived from a cellulose-producing microorganism. The microorganism may be of the genus Acetobacter, Agrobacterium, Rhizobium, Pseudomonas alcaligenes, preferably of the genus Acetobacter, more preferably of the species Acetobacter xylinum or Acetobacter pasteurianus.

[0043] Nanofibrillated cellulose obtained from wood cellulose has been found to be preferred for the medical or scientific products described herein. Wood cellulose is available in large quantities and the preparation methods developed for wood cellulose allow the production of nanofibrillated materials suitable for the products. Nanofibrillated cellulose obtained by fibrillating plant fibers, especially wood fibers, is structurally different and has different properties than nanofibrillated cellulose obtained from microorganisms. For example, compared to bacterial cellulose, nanofibrillated wood cellulose is a homogenous, more porous and free material, which is advantageous in applications involving living cells. Bacterial cellulose is also different in that it is usually used as is, without fibrillation similar to that in plant cellulose. Bacterial cellulose is a dense material that easily forms small spheroids, and the structure of this material is discontinuous, which may make it undesirable to use this material in applications involving living cells, especially when homogeneity of the material is required. In one example, the cellulose is non-bacterial cellulose.

[0044] The wood may be from a softwood tree (such as spruce, pine, fir, larch, Douglas fir, or hemlock), or from a hardwood tree (such as birch, aspen, poplar, alder, eucalyptus, oak, beech, or acacia), or from a mixture of softwood and hardwood. In one example, the nanofibril cellulose is obtained from wood pulp. The nanofibril cellulose may be obtained from hardwood pulp. In one example, the hardwood is birch. The nanofibril cellulose may be obtained from softwood pulp. In one example, the wood pulp is a chemical pulp. Chemical pulps may be desirable for the products disclosed herein. Chemical pulps are pure materials and may be used in a wide range of applications. For example, chemical pulps lack the pitch and resin acids present in mechanical pulps, and are more sterile and easily sterilizable. Furthermore, chemical pulps are more flexible, imparting advantageous properties, for example, in medical and scientific materials, for example, it is possible to prepare highly homogeneous nanofibrillar cellulose materials without the need for excessive processing or specific equipment or cumbersome process steps.

[0045] Nanofibrillar cellulose (including cellulose fibrils and / or fibril bundles) is characterized by a high aspect ratio (length / diameter). The average length of nanofibrillar cellulose (median length of particles such as fibrils or fibril bundles) may be more than 1 μm, and in most cases is less than 50 μm. If the elementary fibrils are not completely separated from each other, the entangled fibrils may have an average total length, for example, in the range of 1 to 100 μm, 1 to 50 μm, or 1 to 20 μm. However, if the nanofibrillar material is highly fibrillated, the elementary fibrils may be completely or almost completely separated and the average fibril length is shorter, for example, in the range of 1 to 10 μm or 1 to 5 μm. This is especially true for native grade fibrils that have not been shortened or digested, for example, chemically, enzymatically or mechanically. However, strongly derivatized nanofibril cellulose may have a shorter average fibril length, for example in the range of 0.3-50 μm, such as 0.3-20 μm, for example 0.5-10 μm or 1-10 μm. In particular, shortened fibrils, such as enzymatically or chemically digested fibrils, or mechanically treated material, may have an average fibril length of less than 1 μm (for example 0.1-1 μm, 0.2-0.8 μm or 0.4-0.6 μm). Fibril length and / or diameter may be estimated by microscopy, for example using CRYO-TEM, SEM or AFM images.

[0046] The average diameter (width) of nanofibril cellulose is less than 1 μm or less than 500 nm (e.g., in the range of 1-500 nm), but preferably less than 200 nm, even less than 100 nm or less than 50 nm (e.g., in the range of 1-200 nm, 2-200 nm, 2-100 nm, or 2-50 nm), and even 2-20 nm for highly fibrillated materials. The diameters disclosed herein may refer to fibrils and / or fibril bundles. The smallest fibrils are on the scale of elementary fibrils, with average diameters typically in the range of 2-12 nm. The dimensions and size distribution of the fibrils depend on the purification method and efficiency. In the case of highly purified native nanofibril cellulose, the average fibril diameter, including fibril bundles, may be in the range of 2-200 nm or 5-100 nm (e.g., in the range of 10-50 nm). Nanofibril cellulose is characterized by a large specific surface area and strong hydrogen bond formation ability. In aqueous dispersion, nanofibril cellulose typically appears as a gel-like material, either light or turbid. Depending on the fiber source, nanofibril cellulose obtained from plants, especially wood, may contain small amounts of other plant components, especially wood components, such as hemicellulose or lignin. The amount depends on the plant source.

[0047] Generally, cellulose nanomaterials can be divided into categories according to TAPPI W13021, which provides standard provisions for cellulose nanomaterials. Not all of these materials are nanofibril cellulose. The two main categories are "nano objects" and "nanostructured materials". Nanostructured materials include "cellulose microcrystals" (sometimes called CMCs) with diameters of 10-12 μm and length:diameter ratios (L / D)<2, and "cellulose microfibrils" with diameters of 10-100 nm and lengths of 0.5-50 μm. Nano objects include "cellulose nanofibers" which can be divided into "cellulose nanocrystals" (CNCs) with diameters of 3-10 nm and L / D>5, and "cellulose nanofibrils" (CNFs or NFCs) with diameters of 5-30 nm and L / D>50. Nanofibril cellulose as disclosed herein can be defined as not being or not containing cellulose microcrystals or nanocrystals.

[0048] The various grades of nanofibrillated cellulose may be categorized based on three main properties: (i) size distribution, length and diameter, (ii) chemical composition, and (iii) rheological properties. Several properties may be used in parallel to fully describe the grades. Examples of the various grades include native (or chemically unmodified) NFC, oxidized NFC (high viscosity), oxidized NFC (low viscosity), carboxymethylated NFC, and cationized NFC. Within these main grades, there are subgrades, e.g.: extremely well fibrillated vs. moderately fibrillated, high vs. low substitution, low vs. high viscosity, etc. The fibrillation technique and chemical pre-modification affect the fibril size distribution. Typically, non-ionic grades have a larger average fibril diameter (e.g., in the range of 10-100 nm or 10-50 nm), while chemically modified grades are significantly thinner (e.g., in the range of 2-20 nm). The distribution is also narrower for modified grades. Certain modifications, particularly TEMPO oxidation, result in shorter fibrils.

[0049] Depending on the raw material source, for example hardwood and softwood pulps, the final nanofibril cellulose products have different polysaccharide compositions. Typically, non-ionic grades are prepared from bleached birch pulp, resulting in a high xylene content (25% by weight). Modified grades are prepared from either hardwood or softwood pulps. In these modified grades, the hemicelluloses are also modified together with the cellulose domains. Almost certainly, this modification is not homogeneous, i.e., some parts are more modified than others. As such, such modified products are complex mixtures of different polysaccharide structures, and detailed chemical analysis is not usually possible.

[0050] In an aqueous environment, dispersions of cellulose nanofibers form viscoelastic hydrogel networks. The gel is already formed at relatively low concentrations, e.g., 0.05-0.2% (w / w), by dispersed and hydrated entangled fibrils. The viscoelastic properties of NFC hydrogels can be characterized, e.g., by dynamic oscillatory rheological measurements.

[0051] Nanofibrillar cellulose hydrogels exhibit distinctive rheological properties. For example, they are shear-thinning or pseudoplastic materials, which may be considered as a special case of thixotropic behavior, meaning that their viscosity depends on the speed (or force) at which the material is deformed. When measuring the viscosity in a rotational rheometer, shear-thinning behavior is seen as a decrease in viscosity with increasing shear rate. Hydrogels exhibit plastic behavior, meaning that a certain shear stress (force) is required before the material begins to flow easily. This critical shear stress is often called the yield stress. Such a yield stress can be determined from a steady-state flow curve measured by a stress-controlled rheometer. When the viscosity is plotted as a function of the applied shear stress, a dramatic viscosity decrease is seen after the critical shear stress is exceeded. Zero shear viscosity and yield stress are the most important rheological parameters to describe the suspension strength of the material. These two parameters allow for a classification of the grades, as they separate the various grades quite clearly.

[0052] The size of the fibrils or fibril bundles can vary depending on, for example, the raw material, Disintegration Method and Disintegration Depends on the number of runs. Cellulosic raw materials Disintegration may be carried out by any suitable equipment, such as a refiner, grinder, disperser, homogenizer, colloider, attrition grinder, pin mill, rotor-rotor disperser, ultrasonic disintegrator, fluidizer (e.g., microfluidizer, macrofluidizer, or fluidizer-type homogenizer, etc.). Disintegration The treatment is carried out under conditions in which sufficient water is present to prevent the formation of interfiber bonds.

[0053] In one example, Disintegration is carried out by using a disperser having at least one rotor, blade, or similar moving mechanical member having at least two rotors (such as a rotor-rotor disperser). In the disperser, the fibrous material in the dispersion is repeatedly impacted by the blades or ribs of the rotor, which strike the material in opposite directions as the blades rotate in opposite directions at a peripheral speed determined by the rotation speed and the radius (distance to the axis of rotation). As the fibrous material is forced radially outward, it breaks on the broad surfaces (i.e., ribs) of the blades, which come one after the other from opposite directions at a peripheral speed; in other words, it receives multiple successive impacts from opposite directions. Furthermore, the edges of the broad surfaces (i.e., ribs) of the blades form a blade gap with the opposite edge of the next rotor blade, which creates a shear force at the edge of the blade, which breaks the fibers. Disintegration and contributes to the detachment of the fibrils. The impact frequency is determined by the rotational speed of the rotors, the number of rotors, the number of blades in each rotor, and the flow rate of the dispersion through the device.

[0054] In rotor-rotor dispersers, fibrous material is introduced radially outwardly with respect to the rotor axis through counter-rotating rotors, where the material is subjected to repeated shear and impact forces by the effect of different counter-rotating rotors and simultaneously fibrillated. An example of a rotor-rotor disperser is the Atrex device.

[0055] Disintegration Other examples of devices suitable for include pin mills, such as multi-peripheral pin mills. One such device includes a housing having a first rotor with an impact surface, a second rotor concentric with the first rotor and with an impact surface, the second rotor being arranged to rotate in the opposite direction to the first rotor, or a stator concentric with the first rotor and with an impact surface. The device has a feed orifice in the housing opening to the centers of the rotors or the centers of the rotors and the stator, and a discharge orifice on the housing wall opening to the periphery of the outermost rotor or stator.

[0056] In one example, Disintegration This is carried out by using a homogenizer, in which the fibrous material is homogenized by the effect of pressure. The homogenization of this fibrous material dispersion into nanofibril cellulose is caused by a forced through-flow of the dispersion, which causes the material to break down into fibrils. Disintegration The fiber material dispersion is passed through a narrow flow-through gap at a given pressure where an increase in the linear velocity of the dispersion induces shear and impact forces on the dispersion, resulting in the removal of fibrils from the fiber material. The fiber fragments are split into fibrils in the fibrillation process. Disintegration will be done.

[0057] As used herein, the term "fibrillation" refers to the mechanical breaking down of fibrous material by the action of particles. Disintegration"Generally refers to the breaking down of the fibers or fiber fragments into smaller particles, whereby the cellulose fibrils are detached from these fibers or fiber fragments. This operation may be based on various effects such as grinding, crushing or shearing, or a combination of these, or another corresponding action that reduces the particle size." Disintegration " or " Disintegration The term "treatment" may be used interchangeably with "fibrillation."

[0058] The fibrous material dispersion to be fibrillated is a mixture of fibrous material and water, also referred to herein as "pulp." A fibrous material dispersion may generally refer to whole fibers, separate portions (fragments) of whole fibers, fibril bundles, or fibrils mixed with water; typically, an aqueous fibrous material dispersion is a mixture of the above elements, with the ratio between the components depending on the degree of processing or processing stages (e.g., the number of runs or "through" the same fibrous material batch through the process).

[0059] One method for characterizing nanofibril cellulose is to use the viscosity of an aqueous solution containing nanofibril cellulose. The viscosity may be, for example, Brookfield viscosity or zero shear viscosity. The specific viscosity described herein differentiates nanofibril cellulose from non-nanofibril cellulose.

[0060] In one example, the apparent viscosity of nanofibril cellulose is measured by a Brookfield viscometer (Brookfield Viscometer) or another equivalent device. Preferably, a vane spindle (number 73) is used. Several commercial Brookfield viscometers for measuring apparent viscosity are available, all based on the same principle. Preferably, an RVDV spring (Brookfield RVDV-III) is used in the device. A sample of nanofibril cellulose is diluted to a concentration of 0.8% by weight in water and mixed for 10 minutes. The diluted sample mass is added to a 250 ml beaker, the temperature is adjusted to 20°C ± 1°C, and heating and mixing are performed if necessary. A low rotation speed of 10 rpm is used. Generally, the Brookfield viscosity can be measured at 20°C ± 1°C, at a consistency of 0.8% (w / w) and at 10 rpm.

[0061] For example, the nanofibril cellulose provided as a starting material in the above method may be characterized by its viscosity in an aqueous solution. The viscosity represents, for example, the degree of fibrillation of the nanofibril cellulose. In one example, the nanofibril cellulose has a Brookfield viscosity of 2000 mPa·s or more (e.g., 3000 mPa·s or more) measured at a consistency of 0.8% (w / w) and 10 rpm at 20°C ± 1°C when dispersed in water. In one example, the nanofibril cellulose has a Brookfield viscosity of 10000 mPa·s or more measured at a consistency of 0.8% (w / w) and 10 rpm at 20°C ± 1°C when dispersed in water. In one example, the nanofibril cellulose has a Brookfield viscosity of 15000 mPa·s or more measured at a consistency of 0.8% (w / w) and 10 rpm at 20°C ± 1°C when dispersed in water. Examples of ranges of Brookfield viscosity (measured at 20°C ± 1°C, 0.8% (w / w) consistency and 10 rpm) of nanofibril cellulose when dispersed in water include 2000-20000 mPa·s, 3000-20000 mPa·s, 10000-20000 mPa·s, 15000-20000 mPa·s, 2000-25000 mPa·s, 3000-25000 mPa·s, 10000-25000 mPa·s, 15000-25000 mPa·s, 2000-30000 mPa·s, 3000-30000 mPa·s, 10000-30000 mPa·s, and 15000-30000 mPa·s.

[0062] Nanofibril cellulose may be characterized by its average diameter (or width) or, in addition to its average diameter, by its viscosity (e.g., Brookfield viscosity or zero shear viscosity) and its yield stress or storage modulus. In one example, nanofibril cellulose suitable for use in the products described herein has an average fibril diameter in the range of 1-200 nm or 1-100 nm. In one example, nanofibril cellulose has an average fibril diameter in the range of 1-50 nm, such as 2-20 nm or 5-30 nm. In one example, nanofibril cellulose has an average fibril diameter in the range of 2-15 nm, such as in the case of (TEMPO) oxidized nanofibril cellulose.

[0063] The fibril diameter may be determined by several techniques, such as by microscopy. Fibril thickness and width distribution may be measured by image analysis of images from a field emission scanning electron microscope (FE-SEM), a transmission electron microscope (TEM), such as a cryo-transmission electron microscope (cryo-TEM), or an atomic force microscope (AFM). In general, AFM and TEM are most suitable for nanofibrillar cellulose grades with a narrow fibril size distribution.

[0064] The rheometric viscosity of nanofibrillar cellulose dispersions can be measured at 22°C by a stress-controlled rotational rheometer (AR-G2, TA Instruments, UK) equipped with a cylindrical sample cup of 30 mm diameter with narrow gap blade geometry (diameter 28 mm, length 42 mm). After loading the sample into the rheometer, the measurement is started after 5 minutes of rest. The steady-state viscosity is measured by gradually increasing the shear stress (proportional to the applied torque) and the shear rate (proportional to the angular velocity). The reported viscosity at a certain shear stress (=shear stress / shear rate) is recorded after a constant shear rate is reached or after a maximum of 2 minutes. When the shear rate is increased to 1000 seconds, the viscosity is measured at 22°C. -1 The measurement is stopped when the viscosity exceeds this value. This method can be used to determine the zero shear viscosity.

[0065] In one example, the nanofibril cellulose provided as a starting material in the above method, when dispersed in water, has a zero shear viscosity (a "plateau" of constant viscosity at low shear stress) measured by a rotational rheometer at a consistency of 0.5% by weight (w / w) in an aqueous solvent at 22°C ± 1°C, in the range of 1000 to 50000 Pa·s (e.g., in the range of 2000 to 20000 Pa·s), and a yield stress (shear stress at which shear thinning begins) in the range of 1 to 30 Pa (e.g., in the range of 3 to 15 Pa). In one example, the nanofibril cellulose has a zero shear viscosity in the range of 5000 to 50000 Pa·s and a yield stress in the range of 3 to 15 Pa. Such nanofibril cellulose may have an average fibril diameter of 200 nm or less (e.g., in the range of 1 to 200 nm).

[0066] In one embodiment, the nanofibril cellulose has an average fibril diameter in the range of 1 to 200 nm, and / or, when dispersed in water, has a storage modulus of 350 Pa or more (e.g., in the range of 350 to 5000 Pa, or preferably 350 to 1000 Pa) and a yield stress of 25 Pa or more (e.g., in the range of 25 to 300 Pa, preferably 25 to 75 Pa) measured by a stress-controlled rotational rheometer under conditions of gradually increasing shear stress in the range of 0.001 to 100 Pa at 25°C, a strain of 2%, and a frequency of 10 rad / sec.

[0067] Turbidity is the cloudiness or haze of a fluid caused by individual particles (i.e., whole suspended or dissolved solids) that are usually not visible to the naked eye. There are several practical ways to measure turbidity, the most direct being some measure of the attenuation (i.e., reduction in intensity) of light as it passes through a sample column of water. An alternatively used Jackson Candle method (units: Jackson Turbidity Units or JTU) is essentially an inverse measure of the length of a column of water required to completely obscure a candle flame when viewed through it.

[0068] Turbidity may be quantitatively measured by using an optical turbidity measuring instrument. There are several commercial turbidity meters available to quantitatively measure turbidity. In the present case, a nephelometric based method is used. The unit of turbidity from a calibrated nephelometer is called Nephelometric Turbidity Units (NTU). The measuring device (turbidimeter) is calibrated and controlled by a standard calibration sample, and then the turbidity of the diluted NFC sample is measured.

[0069] In one turbidity measurement method, a nanofibril cellulose sample is diluted with water to a concentration below the gel point of the nanofibril cellulose and the turbidity of the diluted sample is measured. The concentration at which the turbidity of the nanofibril cellulose sample is measured is 0.1%. A HACH P2100 turbidimeter equipped with a 50 ml measuring vessel is used for the turbidity measurement. The dry content of the nanofibril cellulose sample is measured and 0.5 g of the sample is calculated as the dry content, which is placed in the measuring vessel, filled with tap water to 500 g and mixed vigorously by shaking for about 30 seconds. Without delay, the aqueous mixture is divided into five measuring vessels and these are inserted into the turbidimeter. Three measurements are carried out in each vessel. The mean value and standard deviation are calculated from the obtained results and the final result is given in NTU units.

[0070] One way to characterize nanofibrillated cellulose is to define both viscosity and turbidity. Low turbidity refers to small fibril size (e.g. small diameter) since small fibrils scatter light poorly. Generally, as the degree of fibrillation increases, the viscosity increases and the turbidity decreases at the same time. However, this only occurs up to a certain point. If the fibrillation continues further, the fibrils eventually begin to break and are no longer able to form a strong network. Therefore, from this point on, both the viscosity and turbidity begin to decrease.

[0071] In one example, the turbidity of the anionic nanofibril cellulose, measured by nephelometry at a consistency of 0.1% (w / w) in an aqueous solvent, is less than 90 NTU (e.g., 3 to 90 NTU (e.g., 5 to 60 NTU), such as 8 to 40 NTU). In one example, the turbidity of the native nanofibrils, measured by nephelometry at a consistency of 0.1% (w / w) in an aqueous solvent at 20°C ± 1°C, can be higher than 200 NTU, such as 10 to 220 NTU (e.g., 20 to 200 NTU), such as 50 to 200 NTU. To characterize nanofibril cellulose, the above ranges may be combined with viscosity ranges of nanofibril cellulose (e.g., nanofibril cellulose having a Brookfield viscosity, when dispersed in water, of 2000 mPa·s or more, 3000 mPa·s or more, 5000 mPa·s or more (e.g., 10000 mPa·s or more, such as 15000 mPa·s or more), measured at a consistency of 0.8% (w / w) at 20°C ± 1°C and 10 rpm.

[0072] The nanofibril cellulose may be or may include unmodified nanofibril cellulose. The discharge of unmodified nanofibril cellulose is significantly faster than, for example, anionic grades. Unmodified nanofibril cellulose generally has a Brookfield viscosity measured at 20°C ± 1°C at a consistency of 0.8% (w / w) and 10 rpm in the range of 2000 to 10000 mPa·s. The nanofibril cellulose preferably has a suitable carboxylic acid content, as determined by conductometric titration, in the range of 0.6 to 1.4 mmol COOH / g, for example (for example in the range of 0.7 to 1.2 mmol COOH / g, or in the range of 0.7 to 1.0 mmol COOH / g, or in the range of 0.8 to 1.2 mmol COOH / g).

[0073] DisintegrationThe modified fibrous cellulose raw material may be a modified fibrous raw material. Modified fibrous raw material means a raw material whose fibers are subjected to a treatment such that the cellulose nanofibrils can be more easily detached from said fibers. The modification is usually carried out on fibrous cellulose raw materials present as a suspension in a liquid, i.e. pulp.

[0074] The modification treatments applied to the fibers can be chemical, enzymatic or physical. In chemical modification, the chemical structure of the cellulose molecule is changed by chemical reactions ("derivatization" of the cellulose), preferably resulting in the addition of functional groups to the β-D-glucopyranose units of the polymer, while the length of the cellulose molecule is not affected. The chemical modification of cellulose occurs to a certain degree of conversion, depending on the dosage of the reagents and the reaction conditions, and is generally not complete, so that the cellulose remains in solid form as fibrils and does not dissolve in water. In physical modification, anionic, cationic or non-ionic substances or any combination of these are physically adsorbed on the cellulose surface.

[0075] The cellulose in the fibers may be ionically charged, especially after modification. The ionic charge of the cellulose weakens the internal bonds of the fibers and subsequently leads to the formation of nanofibrillar cellulose. Disintegration The ionic charge may be obtained by chemical or physical modification of the cellulose. The fibers may have a higher anionic or cationic charge after modification compared to the starting material. The most commonly used chemical modification methods to create anionic charges are oxidation, where hydroxyl groups are oxidized to aldehydes and carboxyl groups, sulfonation and carboxymethylation. Chemical modification may be desirable to introduce groups such as carboxyl groups that can participate in the formation of covalent bonds between nanofibril cellulose and bioactive molecules. The cationic charge may then be chemically created by cationization by attaching cationic groups (such as quaternary ammonium groups) to the cellulose.

[0076] Nanofibril cellulose may include chemically modified nanofibril cellulose, which may generally include, for example, anionic or cationic modification. In one example, the nanofibril cellulose is anionically modified nanofibril cellulose. In one example, the nanofibril cellulose is not cationically modified nanofibril cellulose. In one example, the anionically modified nanofibril cellulose is oxidized nanofibril cellulose. In one example, the anionically modified nanofibril cellulose is sulfonated nanofibril cellulose. In one example, the anionically modified nanofibril cellulose is carboxymethylated nanofibril cellulose. Materials obtained by anionic modification of cellulose may be referred to as anionic cellulose, which refers to materials in which the amount or proportion of anionic groups, such as carboxylic acid groups, is increased by such modification compared to the unmodified material. It is also possible to introduce other anionic groups, such as phosphate or sulfate groups, into the cellulose instead of or in addition to the carboxylic acid groups. The content of these groups may be within the same ranges as disclosed herein for carboxylic acids.

[0077] Cellulose may be oxidized. In the oxidation of cellulose, the primary hydroxyl groups of cellulose may be catalytically oxidized, for example, through N-oxyl mediated catalytic oxidation, by heterocyclic nitroxyl compounds, for example, 2,2,6,6-tetramethylpiperidinyl-1-oxy free radical, commonly referred to as "TEMPO". The primary hydroxyl groups (C6-hydroxyl groups) of the cellulose β-D-glucopyranose units are selectively oxidized to carboxylic acid groups. Some aldehyde groups are also formed from the primary hydroxyl groups. A low degree of oxidation does not allow efficient sufficient fibrillation, while a high degree of oxidation results in the formation of cellulose after mechanical disruption treatment. DisintegrationIn view of the finding that this gives rise to the above-mentioned fact, cellulose may be oxidized to a level in which the carboxylic acid content in the oxidized cellulose, as determined by conductometric titration, is within the range of 0.5 to 2.0 mmol COOH / g pulp, 0.6 to 1.4 mmol COOH / g pulp, or 0.8 to 1.2 mmol COOH / g pulp, preferably 1.0 to 1.2 mmol COOH / g pulp. The resulting oxidized cellulose fibers can be dissolved in water to give a carboxylic acid content of 0.5 to 2.0 mmol COOH / g pulp, 0.6 to 1.4 mmol COOH / g pulp, or 0.8 to 1.2 mmol COOH / g pulp, preferably 1.0 to 1.2 mmol COOH / g pulp. Disintegration When subjected to oxidized pulp, it results in a stable, transparent dispersion of individualized cellulose fibrils, which may be, for example, 3-5 nm wide. Using oxidized pulp as the starting medium, it is possible to obtain highly fibrillated nanofibril cellulose with a Brookfield viscosity measured at a consistency of 0.8% (w / w) of 10,000 mPa·s or more (for example in the range of 10,000-30,000 mPa·s).

[0078] Whenever the catalyst "TEMPO" is mentioned in this disclosure, it is clear that all procedures and procedures involving "TEMPO" apply equally and analogously to any derivative of TEMPO or any heterocyclic nitroxyl radical capable of selectively catalyzing the oxidation of the hydroxyl group at the C6 carbon of cellulose.

[0079] The modifications of nanofibrillar cellulose disclosed herein may be applied to other fibrillar cellulose grades described herein, e.g. highly purified cellulose or microfibrillar cellulose may be similarly modified chemically or enzymatically, however there are differences, e.g. in the final degree of fibrillation of these materials.

[0080] In one example, such chemically modified nanofibril cellulose, when dispersed in water, has a Brookfield viscosity of 10000 mPa·s or more, 15000 mPa·s or more, or 18000 mPa·s or more, measured at a consistency of 0.8% (w / w) and 10 rpm at 20° C.±1° C. Examples of anionic nanofibril cellulose used have a Brookfield viscosity in the range of 13000-25000 mPa·s, 13000-20000 mPa·s, or 15000-20000 mPa·s, depending on the degree of fibrillation.

[0081] In one example, the nanofibril cellulose is TEMPO oxidized nanofibril cellulose. The cellulose has a high viscosity at a low concentration, for example, a Brookfield viscosity of 20,000 mPa·s or more, or even 25,000 mPa·s or more, measured at 20°C±1°C, a consistency of 0.8% (w / w), and 10 rpm. In one example, the Brookfield viscosity of the TEMPO oxidized nanofibril cellulose is in the range of 20,000 to 30,000 mPa·s (e.g., 25,000 to 30,000 mPa·s), measured at 20°C±1°C, a consistency of 0.8% (w / w), and 10 rpm.

[0082] Generally, chemically unmodified nanofibril cellulose, when dispersed in water, has a Brookfield viscosity measured at a consistency of 0.8% (w / w) at 20°C ± 1°C and 10 rpm of less than 2000 mPa·s, or greater than 3000 mPa·s.

[0083] Auxiliary agents may be included in the nanofibril cellulose dispersion to enhance the manufacturing process or to improve or adjust the properties of the product. Such auxiliary agents may be soluble in the liquid phase of the dispersion, may form an emulsion, or may be solid. The auxiliary agents may be added to the raw materials already during the production of the nanofibril cellulose dispersion, or may be added to the formed nanofibril cellulose dispersion or gel. The auxiliary agents may be added to the final product, for example, by impregnation, spraying, dipping, soaking, or similar methods. The auxiliary agents are usually not covalently bound to the nanofibril cellulose, and therefore may be releasable from the nanocellulose matrix. Controlled and / or sustained release of auxiliary agents may be obtained when using NFC as a matrix. Examples of auxiliary agents include therapeutic agents (pharmaceuticals) and other agents that affect the properties of the product or the properties of the active agents, such as buffers, surfactants, plasticizers, emulsifiers, etc. In one example, the dispersion contains one or more salts, which may be added to improve the properties of the final product or to aid in the removal of water from the product during the manufacturing process. Examples of salts include chloride salts, such as sodium chloride, calcium chloride, and potassium chloride. The salts may be present in the dispersion in an amount ranging from 0.01 to 1.0% (w / w) of the dry matter. The final product may be immersed or soaked in a solution of sodium chloride, such as about 0.9% aqueous sodium chloride solution. The desired salt content in the final product may be in the range of 0.5 to 1% (such as about 0.9%) of the weight of the wet product. Salts, buffers, and similar agents may be applied to obtain physiological conditions.

[0084] Polyvalent cations may be included to obtain non-covalent crosslinking of the nanofibril cellulose. One example is a nanofibril cellulose product comprising nanofibril cellulose (particularly anionically modified nanofibril cellulose) and polyvalent cations (e.g., polyvalent metal cations selected from calcium, magnesium, zinc, aluminum, gold, platinum and titanium cations), in which the nanofibril cellulose is crosslinked by the polyvalent cations. The amount of polyvalent cations is calculated from the dry content of the hydrogel and may be in the range of 0.1 to 3% (w / w) (e.g., 0.1 to 2% (w / w)).

[0085] One example is a method for preparing such a hydrogel, comprising providing a pulp, mixing the pulp until nanofibril cellulose is obtained. Disintegration and forming the resulting nanofibril cellulose into a hydrogel.

[0086] The nanofibrillated cellulose may be fibrillated to a desired degree of fibrillation and adjusted to a desired water content or otherwise modified to form a gel having the desired properties described herein. In one example, the nanofibrillated cellulose in the hydrogel is anionically modified nanofibrillated cellulose.

[0087] Hydrogels used as medical or scientific hydrogels need to be homogenous. Therefore, the method for preparing a hydrogel may include homogenizing the hydrogel comprising nanofibrillated cellulose, preferably by a homogenizing device such as the one described herein. This preferably non-fibrillating homogenization step makes it possible to remove discontinuous regions from the gel. A homogenous gel is obtained with better properties for these applications. The hydrogel may be further sterilized, for example, by using heat and / or radiation and / or by adding a sterilizing agent, such as an antimicrobial agent.

[0088] Manufacturing of objects The hydrogels disclosed herein may be tailored to fit a particular wound. The moldability or formability of the hydrogels (especially those with a nanofibrillar cellulose content in the range of 2-3.5% (w / w)) allows for the preparation of such preformed or preshaped structures or products that may be tailored to specific requirements. One or more manufacturing device(s), mold(s), and / or other devices or materials may be provided, such as computerized control devices for controlling the manufacturing device(s) and / or process. Providing a preformed or preshaped product may be useful when treating deep wounds where it is not desirable to mold the hydrogel in the wound to avoid deep tissue damage or irritation.

[0089] A preformed structure, which may be a wound dressing, may be manufactured, for example, by molding or by using additive manufacturing, commonly known as 3D printing. Additive manufacturing is a process in which materials are joined or solidified under computer control to create a three-dimensional object. This may be done without a mold. Such materials may be added together layer by layer, for example, by using and controlling one or more nozzles for applying or dispensing the materials.

[0090] In such a method, it may be necessary to obtain information about the three-dimensional structure of the wound or other injury to which the individualized structure is to be applied. The information is used to prepare a digital three-dimensional model of such wound and / or an object designed to fit such wound. Thus, a digital three-dimensional model of the object designed to fit such wound may be obtained and provided. This may be performed by first scanning a target such as a wound or other injury, for example by a 3D scanner or other means for obtaining three-dimensional information of the target, and using the three-dimensional information of the target to create a digital three-dimensional model of the target. The digital three-dimensional model may be configured to generate a desired object, such as an individualized wound dressing, when output by a further manufacturing device. Thus, in one example, the digital three-dimensional model is obtained from a 3D scan of the wound. This three-dimensional model of the wound may include or correspond to the shape of the entire wound or a part thereof.

[0091] therefore, - Providing a medical hydrogel; - obtaining a digital three-dimensional model of an object designed to fit a wound; and - preparing a three-dimensional object from said medical hydrogel according to said digital three-dimensional model by additive manufacturing to obtain a wound dressing tailored to fit said wound.

[0023] A method for preparing a tailored wound dressing is provided, comprising:

[0092] Obtaining information about the three-dimensional structure of a wound or other injury may be performed by using a suitable imaging device, also called a 3D imaging device, capable of producing a three-dimensional image or model of the target, or a system including such an imaging device. The imaging device may be a 3D scanning device. 3D scanning is a process of analyzing a real object or environment to collect data about its appearance, such as its shape and possibly its color. The collected data may then be used to build a digital 3D model. 3D scanning devices may be classified into contact and non-contact types. Since the contact type may not be desirable in the case of wounds, the imaging device used herein is preferably of the non-contact type, which may be passive or active. An active scanner emits sound, radiation or light to probe an object or environment and detects its reflection or radiation passing through such an object. Possible types of emission used include light, ultrasound or x-ray. The active imaging device may be, for example, a 3D laser scanner, such as a time-of-flight, triangulation or conoscopic laser scanner; or a structured light or dimming 3D scanner. The passive imaging device may be, for example, a stereoscopic system, such as one including two cameras, or a photometric system.

[0093] The method may include providing a 3D imaging device and obtaining a digital three-dimensional model of an object designed to fit a wound by using the 3D imaging device.

[0094] The method may include providing an additive manufacturing device such as a 3D printer or other suitable device configured to include or house one or more container(s) for the hydrogel, one or more nozzles or similar dispensing means, one or more actuator(s) for moving the one or more nozzle(s), and one or more control unit(s) for controlling the movement of the one or more nozzle(s) to obtain the desired object by additive manufacturing. The final object may include a shape that either completely or partially corresponds to the shape of the scanned object, such as a wound.

[0095] It is also possible to manufacture wound dressings with a predetermined shape, such as an overall shape arranged to fit one overall shape of a wound. A series of wound dressings with different predetermined shapes, preferably arranged to fit a general shape or type of wound, may be manufactured and / or provided. Digital three-dimensional model(s) may or may not be used, in one example, the three-dimensional model(s) is not obtained by imaging an existing wound or a specific wound, as discussed above. Instead, the three-dimensional model may be created as a general model, for example by computer design. A manufacturing device may also be provided and / or used to prepare such an overall product, including one or more mold(s) for forming the wound dressing(s). A series of overall wound dressings with different shapes may be provided, for example in a kit, preferably packed in sealed packing(s), which may further contain other wound dressings and / or healing product(s).

[0096] The nanofibril cellulose may be applied to a manufacturing device such as a 3D printer in the consistency desired in the final wound dressing. The nanofibril cellulose may be present as a dispersion or hydrogel with a concentration of 1.5-3.5% (w / w), 2.0-3.5% (w / w) or 2.5-3.5% (w / w), or the above concentrations may be lower or higher, and provided in a container (e.g., syringe, ampoule, bottle, tube, cassette, etc.) that may be designed to be attached to the manufacturing device.

[0097] When 3D printing nanofibril cellulose, the process differs from traditional 3D printing processes. Cellulose does not melt when heated, so methods and devices used for printing materials such as plastics, metals, etc. may not be applicable. A specific manufacturing device may have to be used, such as a syringe-based device that may utilize one or more syringes. Such devices are suitable for nanofibril cellulose hydrogel materials, since they are capable of handling and printing liquids, pastes, gels, or slurries. The manufacturing device may include software operably stored in a control unit configured to control the device, or the device may be connected to an external control unit, such as a computer containing the software. The software, and therefore the manufacturing device, may also be configured to use the digital three-dimensional model as a template for manufacturing the three-dimensional object.

[0098] Nanofibril cellulose as a shear-thinning or thixotropic material behaves differently than conventional materials used in additive manufacturing. When shear forces are applied to the material, e.g. when the material is mixed, pressed and / or forced through a nozzle, nanofibril cellulose gel exhibits a thinning behavior, which facilitates the flow of the material to the target. However, after the material is printed or ejected from the manufacturing device, its viscosity returns to its previous, more viscous state. This can be problematic when forming supports with desired medical hydrogel structures, but it can also facilitate the 3D printing process and the formation of such desired structures. For example, the shear-thinning or thixotropy of the hydrogel can provide a suitable open time that allows the material to be shaped and form the desired structure. There is usually no need to control the temperature, e.g. there is no need to heat and / or cool the material for shaping or setting, but the process can be carried out at room or ambient temperature.

[0099] The medical hydrogel structure may be manufactured or printed onto a substrate, which may be metal, plastic or other suitable material, or may be coated with a non-viscous coating, membrane, or the like.

[0100] The dispensed material may need to be dried, precipitated or fixed, and therefore the method may include a drying, precipitation or fixing step. For example, vacuum or pressure and / or freezing and / or heating may be used to form and / or dehydrate the structure. Drying, precipitation or fixing may be performed only on the final structure, or may be repeated two or more times. In additive manufacturing, if performed by applying more than one layer, the material may need to be dried, precipitated or fixed for 10-30 minutes (e.g., about 15 minutes) before applying a new layer. If the layer is applied manually, for example by using a syringe and injection needle, the layer may need to be dried, precipitated or fixed for a longer time (e.g., 30-60 minutes) before applying a new layer.

[0101] The ejection means, such as the nozzle of the production device, may also play an important role. An example of this ejection device is a syringe, and it has been found that it is preferable that a new or unused syringe should be used each time. A needle, preferably a metal needle, may act as the nozzle. The needle may be, for example, an injection needle, such as about a 16 gauge needle, with a nominal inner diameter of 1.194 mm. In general, the nozzle may have an inner diameter in the range of 0.3-3.0 mm (such as 0.3-2.0 mm), for example 0.3-1.5 mm, 0.4-1.5 mm or 0.4-1.3 mm.

[0102] After additive manufacturing, the material (i.e., medical hydrogel) may need to be dried, precipitated, or fixed, for example, for 30 minutes or more, or 60 minutes or more. The medical hydrogel may be stored for at least 2 weeks after production, especially when stored at refrigerator temperatures such as below 10° C. (e.g., 2-10° C. or 4-8° C.). The medical hydrogel may be packed in a hermetic packing.

[0103] The present application provides a wound dressing tailored to fit the wound, comprising a medical hydrogel tailored to fit the wound. Such a product may be obtained by the additive manufacturing method disclosed above. Such a tailored wound dressing is mechanically stable and retains its shape. Being tailored to fit the wound, application of the dressing to the wound does not cause unnecessary pain to the patient or damage the wound. In such a case, there is no need to manually shape the dressing.

[0104] The wound dressing, customized to fit the wound, may contain only or predominantly nanofibril cellulose as disclosed herein. However, for example in the case of large and / or irregularly shaped wounds, it may be possible to include a support portion for the dressing (e.g. an inner portion or a separate layer coated with nanofibril cellulose hydrogel). The support portion does not have to be part of the actual hydrogel and may comprise a material(s) different from the hydrogel (e.g. a reinforcing material such as non-nanofibril cellulose, plastic, or a composite thereof).

[0105] The present application provides kits containing the medical hydrogel packed in one or more sealed package(s) or in one or more application device(s) (e.g., syringe, applicator, pump, tube, etc.), which may include instructions for using the medical hydrogel to induce angiogenesis in a wound and / or to treat a deep wound in the dermis and / or underlying tissue (preferably to induce angiogenesis or for other purposes disclosed herein).

[0106] The kit may further comprise one or more sheets(s) of a medical product comprising gauze and nanofibril cellulose, preferably with a moisture content of less than 10% (w / w), e.g. in the range of 1-10% (w / w) or 5-10% (w / w). Such a product may be used in a treatment method comprising first covering a wound with a medical hydrogel as disclosed herein, incubating, treating or waiting for a period of time, and replacing the medical hydrogel by a different medical product comprising gauze and nanofibril cellulose. In this case, vascularization in the wound may be initiated and after a suitable time, the conditions in the wound are different and a different medical product may be applied to the wound, which then promotes better healing of the already vascularized wound. The first medical product (i.e. the hydrogel) may absorb harmful substances, e.g. microorganisms, impurities, metabolic products, etc., from the wound in a first stage, promoting this healing process and making the wound more susceptible to a second medical product in a second stage of treatment. The kit may include instructions for using the medical hydrogel and one or more sheet(s) of medical product comprising gauze and nanofibrillated cellulose in a treatment method such as for inducing angiogenesis in a wound and / or for treating deep wounds in the dermis and / or in the lingual tissue, preferably for inducing angiogenesis, or for other purposes disclosed herein.

[0107] For example, the above kit - applying said medical hydrogel to a deep wound, for example for a period of time as disclosed herein; - removing medical hydrogel from wounds, and -Applying a medical product comprising gauze and nanofibrillated cellulose to the wound The instructions may include instructions for:

[0108] The medical product comprising gauze and nanofibril cellulose may comprise gauze impregnated with nanofibril cellulose.

[0109] The medical hydrogels disclosed herein may be provided for use in any of the methods disclosed herein, such as a method for treating a wound, in particular a method for treating a deep wound. The method may be a method for inducing angiogenesis. The subject to be treated may be a patient, such as a human or animal subject or patient.

[0110] In one example, the method comprises: - preferably detecting deep wounds of the dermis and / or of the underlying tissue in a subject or detecting a subject in need of treatment of deep wounds of the dermis and / or of the underlying tissue, - providing a medical hydrogel as disclosed herein, - applying a medical hydrogel to said deep wound; The medical hydrogel may be maintained in the wound after application for a period of time sufficient to impart angiogenesis and / or other healing effects in the wound or tissue(s) of the wound. This period may be, for example, at least 1, 2, 3, 4, or 5 days, up to 7, 10, or 14 days, such as 1-7 days, 1-5 days, 1-4 days, 1-3 days, 1-2 days, 2-14 days, 2-7 days, such as 1-14 days, or 6-168 hours, such as 12-168 hours or 24-168 hours, and in some cases 6-48 hours, such as 6-24 hours or 6-12 hours.

[0111] After said period, the medical hydrogel may be removed from the wound and a second wound dressing may be applied to the wound. The second wound dressing may comprise nanofibril cellulose, but may be of a different type. The second wound dressing may comprise a layer of nanofibril cellulose (preferably a layer of gauze) or may comprise gauze impregnated with nanofibril cellulose. The second wound dressing may be maintained on the wound for at least 6 hours or at least 12 hours or 24 hours, or at least 1 day, 2 days, 3 days, 4 days or 5 days, up to 7 days, for example 12 to 168 hours, 12 to 72 hours, 12 to 48 hours or 6 to 24 hours. One or more further wound dressing(s) may be applied after the previous wound dressing is removed. After the medical hydrogel has been removed from the wound, such as by surgical methods, e.g., by application of a skin graft and / or suture(s), the wound may be treated again with a similar new or unused hydrogel or with other material(s) and / or method(s).

[0112] In one example, the method comprises: - preferably detecting deep wounds of the dermis and / or of the underlying tissue in a subject or detecting a subject in need of treatment of deep wounds of the dermis and / or of the underlying tissue, - providing a medical hydrogel as disclosed herein, - applying a medical hydrogel to a deep wound, preferably for a period of time as disclosed herein; - Removing the medical hydrogel from the wound, and - applying gauze and medical products containing nanofibril cellulose (e.g. gauze impregnated with nanofibril cellulose) to the wound; Includes.

[0113] The present application also provides a medical hydrogel for use in the above method. EXAMPLES

[0114] Example 1 The potential of NFC-derived biomaterials, particularly anionic NFC (ANFC), to provide an optimal scaffold for hASCs, as well as whether hASCs and ANFC together promote wound healing, was studied in vivo in a splinted full-thickness excisional skin wound model in healthy mice before proceeding to a chronic wound model. In this model, the wound is surrounded by a silicone ring attached to the skin by sutures, preventing wound contraction. This model mimics the human wound healing process, where wound repair proceeds mainly via granulation tissue formation and re-epithelialization. The aim was to avoid using additional adhesion proteins for cell transplantation. For this study, ANFC was tested together with native NFC. Although the safety of NFC dressing materials has been proven in previous studies, the native NFC dressing was also shown to improve the uneven distribution of newly formed skin structures (Figure 1).

[0115] Figure 1 shows the histopathological evaluation of wounds in humanized mice treated with NFC dressings (type 1 dressings). Figure 1A shows the case of an untreated injury (animal 71NT), where the dermis begins to appear as small, thin, disorganized collagen fibers filled with inflammatory cell infiltrates. The subcutaneous tissue is present with a small number of adipocytes and also contains immune cell infiltrates. Immune inflammatory cells are also present in the disorganized muscular layer, covering the entire area. This indicates that while the initial process of regeneration is initiated in the lower layers as expected, regeneration is accompanied by acute inflammation in all layers of the skin. Figure 1B shows the case of a type 1 dressing-treated injury (animal 71T), where the dermis contains parallel organized collagen fibers and there is abundant immune cell infiltration in all dermal layers. The subcutaneous tissue has fat cells and is beginning to organize with some collagen fibers, but in parallel with healing and organization with fat cells filled by collagen fibers, it still contains inflammatory and immune cells, but some blood cells are still around. The muscle is healing and filling without stopping the immune cell infiltration. Ar: artery; Col: collagen; Ep: epidermis; Hp: fat-containing subcutaneous tissue; IIC: inflammatory infiltrating cells; Ms: muscle; V: vein.

[0116] In the wound healing experiments to study the effect of ANFC and hASC on the healing process and the suitability of ANFC as a cell scaffold, mice were anesthetized with isoflurane (4-5% at 5 l / min for induction and 1-2% at 1 l / min for maintenance during surgery). The hair on the back of the animals was removed approximately 2 cm on either side of the spine. 2 The area was shaved and the skin was disinfected with chlorhexidine. Two 6 mm full-thickness wounds were made on the shaved dorsal surface, approximately 0.5 cm from the spine on one side and at the level of the rib cage, using a biopsy punch. A silicone ring was then sutured on the surface of the skin surrounding the incision using eight sutures to prevent wound contraction. All reagents and materials used in this animal study were prepared using aseptic techniques.

[0117] Mice were divided into different study groups using randomization (N=4 / group / time point). A "sham" group treated with PBS served as control. Sample sizes for all groups were calculated as follows:

[0118] Chance to conclude that the outcome is different from that in the absence of treatment (Type 1 error rate) = 5% Coefficient of variation (CV) = 15% Expected or detectable effect size (d) = 25% Number of replicates (r) = 15.7*(CV / d) 2 , therefore, r=5.65=6.

[0119] Six wounds were prepared per treatment group. Two wounds were made on each animal, so four animals were needed per treatment group. Four treatments were analyzed at three time points: 4 animals x 3 groups x 3 time points = 36 animals. Treatments were performed by feeding healthy mice (n = 36) (n = 12 / group x 3 groups). These animals were assigned to treatment groups or sham controls of the treatment group (n = 12), ANFC (n = 12) and hASC (n = 12). hASC alone were injected as a local treatment onto the wound bed (100 μl, 1 x 10 7 cells / wound area (cm 2 )).

[0120] After treatment induced wounds, the wounds were protected with transparent film and gauze and covered with an elastic bandage tied around the animal's body. Animals were housed in a warm environment and monitored and scored daily according to the Mouse Grimace scale and a modified score sheet agreed upon by the designated veterinarian prior to the start of the study.

[0121] The progress of wound healing was observed and photographed, and the wound healing rate was calculated until the wound was closed. On days 3, 7, and 21, the mice were anesthetized, and rectangular specimens were excised from the wound, divided into halves, and used for histological studies or tissue protein lysate preparation. After this procedure, the animals were sacrificed.

[0122] Histological skin samples were fixed overnight in 10% formalin at +4°C, washed, cleared in xylene and embedded in paraffin. Samples in paraffin were sectioned using a microtome, mounted on glass slides and immunohistochemically stained. Hematoxylin and eosin (H&E) staining was used to assess re-epithelialization and Masson's trichrome staining to assess granulation tissue formation. Specific marker antibodies were used for staining to examine the expression of proliferation nuclear antigen (PCNA) to detect epidermal closure (keratin K14) and epidermal proliferation. Angiogenesis is examined by staining samples with endothelial cell markers CD31 and α-smooth muscle actin (α-SMA) to detect vascular networks. Infiltration of immune cells into the wound was examined using antibodies against F4.80 and Gr-1 to detect macrophages and neutrophils, respectively. Transplanted hASCs were detected using an antibody against human nuclear antigen (HNA) to examine their integration into the host tissue. To investigate the paracrine secretion of GFs from hASCs in vivo, GFs including VEGF, FGF2 and HGF were examined by double staining with appropriate antibodies along with HNA to demonstrate the biological activity of hASCs in host tissues.

[0123] To prepare tissue protein lysates, tissue samples were snap frozen in liquid nitrogen and then homogenized in RIPA buffer containing protease and phosphatase inhibitors. Protein lysates were subjected to Western blot analysis to examine the expression of GFs, including VEGF, FGF2, and HGF, normalized to β-actin expression, to further confirm the paracrine signaling mechanism of hASCs.

[0124] Statistical differences between two groups were evaluated by Student's t test and comparisons between three or more groups by one-way analysis of variance (ANOVA) followed by Tukey's multiple comparison test. Correlations between different data sets were analyzed by Spearman correlation test.

[0125] result In the experiments performed, anionic nanofibril cellulose (ANFC) hydrogel was shown to promote wound coverage compared to non-chemically modified nanofibril cellulose (GrowDex) and control samples (no treatment), as shown in Figure 2. In particular, the effect of this material on pre-vascularization in wounds was investigated, which is desirable in deep wounds, such as those at or below the dermis.

[0126] In addition to wound coverage, a-SMA staining on day 7 (d7) of the experiment showed that ANFC hydrogel stimulated fibroblast activation compared to control samples (Figure 3). This staining was evident in wounds treated with 3.2% (w / w) anionic nanofibril cellulose, but not with non-chemically modified nanofibril cellulose (GrowDex). Therefore, based on these experiments, it can be concluded that ANFC hydrogel is beneficial for fibroblast activation, resulting in angiogenesis in the tissue.

[0127] Figure 3 shows the results from the stimulation of fibroblast activation. As shown in Figure 3, it can be seen that 3.2% (w / w) anionic nanofibril cellulose (ANFC) hydrogel stimulates fibroblast activation more than non-chemically modified nanofibril cellulose and control samples (no treatment). Figure 3A shows fibroblast activation in various materials at day 7 (d7) of α-SMA staining. Figure 3B is a graph showing α-SMA staining intensity in various materials.

[0128] Comparative studies showed that an anionic nanofibril cellulose hydrogel containing 5.3% (w / w) nanofibril cellulose did not show angiogenic effects and the hydrogel tended to dry out. However, a similar hydrogel containing 2.65% (w / w) nanofibril cellulose enhanced pre-vascularization and the material remained moist. In general, a proportion of about 3% (w / w) was found to be advantageous, and therefore most studies were carried out with a nanofibril cellulose concentration of about 3.2% (w / w).

[0129] However, the moldability of the hydrogel decreases if the gel concentration is too low. Nanofibril cellulose concentrations below 1% (w / w) are not very useful, especially when additive manufacturing is used, as the printability of the material is poor. Concentrations of 2% (w / w) and above are often advantageous in terms of additive manufacturing.

[0130] In summary, NFC hydrogel and its derivatives are valuable scaffold materials by promoting hASC cell growth and properties in culture. NFC-based dressings promote the bioactivity of host tissues and facilitate tissue repair. By promoting wound healing, NFC hydrogels and / or dressings are new and efficient treatments for wound healing.

[0131] Example 2: Chicken study The moldability and stability of various hydrogels were examined using pieces of chicken meat as test subjects. Large, deep wounds were made in the chickens and covered with nanofibrillar cellulose hydrogels. NFC lots 11428 and 11473 were applied to the wounds.

[0132] An anionic nanofibrillated cellulose hydrogel containing 3.27% (w / w) NFC was molded into a wound by manual tapping (Figure 4A) and almost completely removed from the wound. The shape of the removed gel reproduced the shape of the wound (Figure 4B). However, the gel structure was slightly disrupted and small pieces remained in the wound, but could be easily washed away with water. This gel was more resistant to external water than the 2.65% gel.

[0133] An anionic nanofibril cellulose hydrogel containing 2.65% (w / w) NFC could be smoothly molded into the wound with very little tapping (Figure 5A). However, this gel was difficult to remove from the wound because it was sticky and adhesive. The shape of the removed gel (Figure 5B) did not reproduce the shape of the wound as well as the 3.27% gel above. The material remaining in the wound could be washed away with copious amounts of water.

[0134] Example 3: Measurements Rheological measurements Rheological measurements were performed at 37°C with a HAAKE Viscotester iQ Rheometer (Thermo Fisher Scientific, Karlsruhe, Germany) equipped with a Peltier system for temperature control. Results were analyzed by HAAKE RheoWin4.0 software (Thermo Fisher Scientific). A parallel 35 mm diameter steel plate-plate configuration was used with a 1 mm gap in all measurements. The samples were allowed to rest for 5 min at 37°C before each measurement. Controlled stress amplitude sweeps were performed to determine the linear viscoelastic region for the various NFC hydrogel formulations. A constant angular frequency ω = 1 Hz and an oscillatory stress between 0.0001 and 500 Pa were used in all amplitude sweeps. The oscillatory stress selected for the frequency sweep was τ = 50 Pa. Shear viscosity was measured by increasing the shear rate from 0.1 to 1000 (1 / s).

[0135] The shear viscosity (at its own concentration) of 3.2% (w / w) anionic nanofibril cellulose was measured at a shear rate of 0.1 (1 / s), and the viscosity value was 1750 Pa·s.

[0136] water retention content The water retention was measured according to the following procedure.

[0137] ÅAGWR (Åbo Akademi Gravitometric Water Retention) is a coating colour static water retention method developed by Åbo Akademi. ÅAGWR-Hydrogel is a hydrogel water retention capacity method developed for ÅAGWR devices.

[0138] The amount of liquid phase of the sample that passed through the membrane foil at a given time and pressure was measured, and the amount of water absorbed by the hydrogel was calculated.

[0139] The above measurements were performed using an ÅAGWR device, which includes a metal cylinder, a balancing plug, and a rubber measuring platform. A Whatman 17CHR blotting board and a Whatman Nucleopore 0.4 μm membrane foil (diameter 47 mm) were used, as well as a stopwatch and an analytical balance (precision 0.0001 g).

[0140] The dry content of the hydrogel was determined by keeping the sample in an oven at a temperature of 105° C. for 4 hours. The weight of the hydrogel was determined before and after drying. The blotting board was cut into 57 mm×57 mm pieces.

[0141] The measurement procedure was as follows.

[0142] Mix the hydrogel to be measured thoroughly with a spoon. Connect the compressed air and adjust the measuring pressure of the ÅAGWR device to 0.5 bar. Place two equilibrated blotting board pieces with the wire side facing up on the rubber measuring platform. Place the membrane foil with the shiny side facing up on the blotting board. Place the metal cylinder on the filter.

[0143] Approximately 5 g of hydrogel is placed in the cylinder and the equilibration plug is placed in the graduated cylinder for a few seconds to allow it to face-coat against the membrane. The rubber measuring platform is placed on the measuring platform of the device together with the filter and cylinder, and the measuring platform is lifted (CYLINDER).

[0144] The rubber plug is put in place, the pressure is connected (PRESSURE) and the stopwatch is started. The pressure is allowed to interact for 3 minutes, then the pressure is stopped (PRESSURE), the measuring platform is lowered (CYLINDER) and the rubber measuring platform is removed from the measuring platform. The cylinder is removed from the blotting board together with the membrane foil and the blotting board is weighed to the nearest 0.1 g.

[0145] Two parallel measurements are carried out. If the test results differ from each other by more than 5%, further parallel measurements (maximum 3 measurements / sample) are carried out.

[0146] Calculation and reporting of results

number

[0147] The results of the hydrogel water retention capacity test are the average of two parallel measurements. The measurement precision is 0.1 g / g. If the test results differ from each other by more than 5%, further parallel measurements (maximum 3 measurements / sample) are carried out.

[0148] For a 3.2% (w / w) anionic nanofibrillar cellulose hydrogel, a water retention value of 28.5 g water per gram of dry hydrogel was measured, which proved to be particularly advantageous in tests for application to deep wounds to induce angiogenesis. The present invention includes the following aspects. <1> Providing an anionically modified pulp (e.g., wood pulp, etc.) or providing a pulp (e.g., wood pulp, etc.) and anionically modifying the pulp; defibrating the anionically modified pulp until nanofibril cellulose having an average fibril diameter of 200 nm or less is obtained; homogenizing the disintegrated anionically modified pulp in one or more non-fibrillating homogenization steps; The nanofibril cellulose is made into a moldable medical hydrogel having a nanofibril cellulose content in the range of 2 to 3.5% (w / w) (e.g., 2.5 to 3.5% (w / w)) and a viscosity measured by a viscometer at 37°C and a shear rate of 0.1 1 / sec at the hydrogel concentration in the range of 500 to 2200 Pa s (e.g., 700 to 1800 Pa s); 16. A method for preparing a moldable medical hydrogel comprising: <2> A moldable medical hydrogel comprising nanofibril cellulose, the content of the nanofibril cellulose in the hydrogel being within the range of 2 to 3.5% (w / w), the nanofibril cellulose comprising anionic nanofibril cellulose having an average fibril diameter of 200 nm or less, and the viscosity of the hydrogel measured by a viscometer at 37°C at a shear rate of 0.1 1 / sec at the concentration of the hydrogel being within the range of 500 to 2200 Pa s. <3> The content of nanofibril cellulose in the hydrogel is within the range of 2.5 to 3.5% (w / w); <2> A moldable medical hydrogel according to claim 1. <4> The hydrogel has a viscosity measured by a viscometer at a shear rate of 0.1 1 / sec at a concentration of the hydrogel and at 37°C, within the range of 700 to 1800 Pa s. <2> or <3> A moldable medical hydrogel according to claim 1. <5> The nanofibril cellulose has a water retention value measured by the ÅAGWR (Åbo Akademi Gravitometric Water Retention) method in the range of 20 to 70 g of water per 1 g of dry hydrogel (preferably 23 to 50 g of water per 1 g of dry hydrogel). <2> ~ <4> 13. A moldable medical hydrogel according to any one of claims 1 to 12. <6> The nanofibril cellulose, when dispersed in water, has a zero shear viscosity in the range of 1000 to 50000 Pa s (e.g., in the range of 2000 to 20000 Pa s) and a yield stress in the range of 1 to 30 Pa (e.g., in the range of 3 to 15 Pa), as measured by a rotational rheometer at a consistency of 0.5% by weight (w / w) in an aqueous solvent at 22°C ± 1°C. <2> ~ <5> 13. A moldable medical hydrogel according to any one of claims 1 to 12. <7> <1> 2. The method according to claim 1, <2> ~ <6> 13. A moldable medical hydrogel according to any one of claims 1 to 12. <8> For use in inducing angiogenesis in wounds (such as deep wounds in the dermis and / or underlying tissues), <2> ~ <7> 13. A moldable medical hydrogel according to any one of claims 1 to 12. <9> For use in treating wounds (such as deep wounds in the dermis and / or underlying tissue) to activate fibroblasts; <2> ~ <7> 13. A moldable medical hydrogel according to any one of claims 1 to 12. <10> For use in treating deep wounds of the dermis and / or underlying tissue (e.g., for activating fibroblasts) by the following method: <2> ~ <7> The moldable medical hydrogel according to any one of claims 1 to 5, The method further comprising: applying a moldable medical hydrogel to a deep wound, preferably for 6 hours or more, 12 hours or more, or 24 hours or more; removing the moldable medical hydrogel from the wound; and applying a medical product comprising gauze and nanofibril cellulose (such as gauze impregnated with nanofibril cellulose) to the wound; The moldable medical hydrogel comprising: <11> <2> ~ <10> Providing a moldable medical hydrogel according to any one of the above claims, Obtaining a digital three-dimensional model of an object designed to fit the wound; and Preparing a three-dimensional object from said medical hydrogel according to said digital three-dimensional model by additive manufacturing to obtain a wound dressing tailored to fit said wound. 16. A method for preparing a tailored wound dressing comprising: <12> The digital three-dimensional model is obtained from a 3D scan of the wound. <11> The method according to <13> A wound dressing tailored to fit the wound, preferably <11> or <12> 2. A wound dressing adapted to the wound, obtained by the method according to claim 1 . <2> ~ <10> The wound dressing comprises the moldable medical hydrogel according to any one of claims 1 to 5. <14> packed in one or more sealed packages or in one or more application devices (such as syringes, applicators, pumps or tubes) <2> ~ <10> A kit comprising the moldable medical hydrogel described in any one of claims 1 to 5. <15> Further comprising one or more sheets of gauze and nanofibril cellulose-containing medical products (such as gauze impregnated with nanofibril cellulose), preferably with a moisture content of less than 10% (w / w); <14> The kit according to claim 1,

Claims

1. Providing an anionic chemically modified pulp or providing a pulp and anionic chemically modifying the pulp; defibrating the anionic chemically modified pulp until a hydrogel containing anionic chemically modified nanofibril cellulose having an average fibril diameter of 200 nm or less is obtained; homogenizing the hydrogel comprising anionic chemically modified nanofibrillary cellulose obtained from the disaggregated anionic chemically modified pulp in one or more non-fibrillating homogenization steps; The anionic chemically modified nanofibril cellulose is a hand-formable medical hydrogel having a nanofibril cellulose content in the range of 2.0 to 3.5% (w / w), and a viscosity of the hydrogel at a shear rate of 0.1 1 / sec and 37°C measured by a viscometer is in the range of 500 to 2200 Pa·s.

16. A method for preparing a hand moldable medical hydrogel, comprising:

2. 2. The method of claim 1, comprising preparing a hand moldable medical hydrogel from the anionic chemically modified nanofibril cellulose, the nanofibril cellulose content being in the range of 2.5-3.5% (w / w).

3. The method according to claim 1 or claim 2, comprising producing a hand moldable medical hydrogel from the anionic chemically modified nanofibril cellulose, the viscosity of which is within the range of 1000 to 2000 Pa·s at a shear rate of 0.1 1 / sec at 37°C at the concentration of the hydrogel as measured by a viscometer.

4. A hand-moldable medical hydrogel comprising nanofibril cellulose, the content of the nanofibril cellulose in the hydrogel being within the range of 2.0 to 3.5% (w / w), the nanofibril cellulose comprising anionic chemically modified nanofibril cellulose having an average fibril diameter of 200 nm or less, and the hydrogel having a viscosity, measured by a viscometer at 37°C and a shear rate of 0.1 1 / sec at the concentration of the hydrogel, within the range of 500 to 2200 Pa·s.

5. The hand moldable medical hydrogel of claim 4, wherein the content of nanofibril cellulose in the hydrogel is within the range of 2.5 to 3.5% (w / w).

6. The hand moldable medical hydrogel according to claim 4 or claim 5, wherein the hydrogel has a viscosity in the range of 1000 to 2000 Pa·s as measured by a viscometer at a shear rate of 0.1 1 / sec at 37°C at the concentration of the hydrogel.

7. The hand moldable medical hydrogel according to any one of claims 4 to 6, wherein the nanofibril cellulose has a water retention value measured by the ÅAGWR (Åbo Akademi Gravitometric Water Retention) method in the range of 20 to 70 g of water per gram of dry hydrogel.

8. The hand moldable medical hydrogel of any one of claims 4 to 7, wherein the nanofibril cellulose, when dispersed in water, has a zero shear viscosity in the range of 1000 to 50000 Pa s and a yield stress in the range of 1 to 30 Pa, as measured by a rotational rheometer at a consistency of 0.5 weight percent (w / w) in an aqueous solvent at 22°C ± 1°C.

9. The hand moldable medical hydrogel of any one of claims 4 to 8, wherein the nanofibril cellulose, when dispersed in water, has a zero shear viscosity in the range of 2000 to 20000 Pa s and a yield stress in the range of 3 to 15 Pa, as measured by a rotational rheometer at a consistency of 0.5% by weight (w / w) in an aqueous solvent at 22°C ± 1°C.

10. A hand moldable medical hydrogel according to any one of claims 4 to 9 for use in inducing angiogenesis in deep wounds of the dermis and / or underlying tissue.

11. A hand moldable medical hydrogel according to any one of claims 4 to 10 for use in treating deep wounds in the dermis and / or underlying tissue by activating fibroblasts.

12. 12. A hand moldable medical hydrogel according to any one of claims 4 to 11 for use in a method for treating deep wounds of the dermis and / or underlying tissue by activating fibroblasts, comprising: The method further comprising: applying a moldable medical hydrogel to the deep wound and maintaining the application to said deep wound for a period of 6 hours to 168 hours; removing the moldable medical hydrogel from the wound; and applying to said wound a medical product comprising gauze having a moisture content of less than 10% (w / w) and impregnated with nanofibrillated cellulose; The moldable medical hydrogel comprising:

13. Providing a hand moldable medical hydrogel according to any one of claims 4 to 12, Obtaining a digital three-dimensional model of an object designed to fit the wound; and Preparing a three-dimensional object from the medical hydrogel according to the digital three-dimensional model by additive manufacturing to obtain a wound dressing tailored to fit the wound.

16. A method for preparing a tailored wound dressing comprising:

14. The method of claim 13, wherein the digital three-dimensional model is obtained from a 3D scan of the wound.

15. A kit comprising the moldable medical hydrogel of any one of claims 4 to 12 packed in one or more sealed packages or in one or more application devices selected from a syringe, an applicator, a pump and a tube.

16. 16. The kit of claim 15, further comprising one or more sheets of medical product comprising gauze impregnated with nanofibrillar cellulose, the gauze having a moisture content of less than 10% (w / w).

Citation Information

Patent Citations

  • Method for producing a medical product containing nanofibril cellulose, and medical product

    JP2019514461A

  • Nanofibrillar polysaccharide for use in the control and prevention of contraction and scarring

    US20150367024A1

  • Medical hydrogel

    WO2018109275A1