Method for manufacturing transparent conductive substrate, transparent conductive substrate
The method addresses the challenges of high resistance and reflectance in transparent conductive substrates by using a laminate structure with nickel and copper layers and distinct etching solutions, resulting in a substrate with reduced reflectance and improved conductivity for capacitive touch panels.
Patent Information
- Application Number
- JP2019522085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-07-25
- Filing Date
- 2018-05-14
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2038-05-14
AI Technical Summary
Existing transparent conductive substrates used in capacitive touch panels face issues with high electrical resistance and visibility due to the use of ITO, which is unsuitable for large panels, and metal wiring reflects light, reducing display visibility.
A method for manufacturing a transparent conductive substrate involving a laminate structure with a first blackening layer containing nickel and copper, a conductive layer, and a second blackening layer, using distinct etching solutions to pattern these layers, ensuring the blackening layer is etched without residue and the conductive layer maintains integrity.
The method allows for the production of a transparent conductive substrate with reduced reflectance and improved adhesion, enabling effective patterning of the blackening layer into desired shapes without residue, enhancing display visibility and conductivity.
Smart Images

Figure 0007568399000009 
Figure 0007568399000010 
Figure 0007568399000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a transparent conductive substrate, and a transparent conductive substrate. [Background technology]
[0002] A capacitive touch panel detects changes in capacitance caused by an object approaching the panel surface, and converts the position information of the object on the panel surface into an electrical signal. The transparent conductive substrate used in a capacitive touch panel is placed on the surface of a display, so the wiring material of the transparent conductive substrate is required to have low reflectance and to be difficult to see.
[0003] Therefore, a material with low reflectance and low visibility is used as the wiring material for the capacitive touch panel, and the wiring is formed on a transparent substrate or a transparent film. For example, Patent Document 1 discloses a transparent conductive film for touch panels in which an ITO (indium tin oxide) film is formed as a transparent conductive film on a polymer film.
[0004] In recent years, displays equipped with touch panels have become larger in size, and accordingly, transparent conductive substrates such as transparent conductive films for touch panels are required to have larger areas. However, ITO has a high electrical resistance and causes signal degradation when the wiring length becomes long, making it unsuitable for large panels.
[0005] For this reason, the use of metal wiring made of copper or the like instead of ITO has been considered, as disclosed in, for example, Patent Documents 2 and 3. However, the metal used for the metal wiring has a metallic luster, which causes a problem of reduced visibility of the display due to reflection.
[0006] Therefore, it has been considered to form a blackening layer on a conductive layer made of a metal material on a transparent substrate, the blackening layer suppressing light reflection on the surface of the conductive layer, and then pattern the conductive layer and the blackening layer to create a transparent conductive substrate in which a blackening layer is formed on the surface of the metal wiring. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2003-151358 [Patent Document 2] Japanese Patent Application Publication No. 2011-018194 [Patent Document 3] Japanese Patent Application Publication No. 2013-069261 Summary of the Invention [Problem to be solved by the invention]
[0008] The inventors of the present invention have investigated a transparent conductive substrate including a blackened layer containing nickel and copper as a transparent conductive substrate capable of particularly suppressing light reflection on the surface of a conductive layer using a metal material. Specifically, the inventors have investigated a transparent conductive substrate including a laminate in which a first blackened layer containing nickel and copper, a conductive layer using a metal material containing copper, and a second blackened layer containing nickel and copper are laminated in that order from the transparent substrate side.
[0009] By the way, in order to manufacture a transparent conductive substrate having a wiring pattern by patterning a laminate substrate in which a laminate including a blackening layer and a conductive layer is arranged on a transparent base material, a resist having an opening of a shape corresponding to the part to be removed by etching is arranged on the surface of the laminate. Then, an etching solution capable of etching both the blackening layer and the conductive layer is supplied to etch the laminate including the blackening layer and the conductive layer. After that, the resist is peeled off and removed to manufacture a transparent conductive substrate having a wiring pattern. As described above, in the past, the blackening layer and the conductive layer were etched with the same etching solution from the viewpoint of productivity.
[0010] However, when the blackening layer and the conductive layer are etched with a single etching solution, there was a problem in that the blackening layer in contact with the transparent base material (in the case of the above-mentioned configuration, the first blackening layer) was partially left undissolved after etching, making it easy for residue to be generated.
[0011] In particular, in recent years, when a transparent conductive substrate is mounted on a display, there has been a demand for a blackening layer that can further suppress the reflectance on the conductive layer surface in order to make the wiring pattern less noticeable.
[0012] In the case of a blackening layer containing nickel and copper, the reflectance on the surface of the conductive layer can be further suppressed by increasing the content of nickel oxide. However, nickel oxide has low reactivity with an etching solution that can etch both the blackening layer and the conductive layer, such as an etching solution such as ferric chloride, so that suppressing the reflectance makes it easier for residues of the blackening layer to be generated, and the blackening layer cannot be patterned into a desired shape.
[0013] In view of the above problems in the conventional technology, an object of one aspect of the present invention is to provide a method for producing a transparent conductive substrate, which is capable of patterning a blackening layer into a desired shape. [Means for solving the problem]
[0014] In order to solve the above problem, one aspect of the present invention is to A transparent substrate; and a layer of nickel, copper, nickel oxide, and copper oxide disposed on at least one surface of the transparent substrate. Consisting only of a patterning step of patterning a laminate substrate including a laminate in which a first blackening layer and a copper-containing conductive layer are laminated in this order from the transparent base material side, The patterning process includes a conductive layer etching step of etching the conductive layer with a first etching solution capable of dissolving copper; and a first blackening layer etching step of etching the first blackening layer with a second etching solution containing chloride ions and water, wherein the second etching solution has a chloride ion concentration of 10 mass % or more calculated as hydrochloric acid. Effect of the Invention
[0015] According to one aspect of the present invention, there is provided a method for producing a transparent conductive substrate, which is capable of patterning a blackening layer into a desired shape. [Brief description of the drawings]
[0016] [Figure 1A] FIG. [Figure 1B] FIG. [Figure 2A] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 2B] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 2C] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 2D] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 3A] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 3B] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 3C] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 3D] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 3E] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 4A] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 4B] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 4C] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Figure 4D] 1A to 1C are explanatory views of a method for producing a transparent conductive substrate according to an embodiment of the present invention. [Diagram 5] FIG. 2 is an explanatory diagram of a transparent conductive substrate having mesh-like wiring. [Figure 6A] An example of the cross-sectional view taken along line AA' in Figure 5. [Figure 6B] An example of the cross-sectional view taken along line AA' in Figure 5. [Figure 7A] FIG. 2 is an explanatory diagram of a transparent conductive substrate according to an embodiment of the present invention. [Figure 7B] FIG. 2 is an explanatory diagram of a transparent conductive substrate according to an embodiment of the present invention. [Figure 8] 1 is an electron microscope photograph of a transparent conductive substrate including lattice-shaped thin metal wires obtained in Experimental Example 4-1. [Figure 9] 4 is an electron microscope photograph of a conductive wiring layer portion of the transparent conductive substrate obtained in Experimental Example 7-1. [Figure 10] 1 is an electron microscope photograph of a conductive wiring layer portion of the transparent conductive substrate obtained in Experimental Example 7-6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, one embodiment of the method for producing a transparent substrate of the present invention will be described.
[0018] The method for producing a transparent conductive substrate of this embodiment can include a patterning step of patterning a laminate substrate including a transparent substrate, and a laminate disposed on at least one surface of the transparent substrate, the laminate being formed by laminating a first blackening layer containing nickel and copper, and a conductive layer containing copper, in that order from the transparent substrate side. And the patterning process can further include the following steps:
[0019] A conductive layer etching step of etching the conductive layer with a first etching solution capable of dissolving copper. A first blackened layer etching step of etching the first blackened layer with a second etching solution containing chloride ions and water. The second etching liquid may have a chloride ion concentration of 10 mass % or more calculated as hydrochloric acid.
[0020] First, each member included in the laminate substrate used in the method for producing a transparent conductive substrate of this embodiment will be described below.
[0021] The transparent substrate is not particularly limited, and for example, a resin substrate (resin film) or a glass substrate that transmits visible light can be preferably used.
[0022] As the material of the resin substrate that transmits visible light, for example, polyamide resin, polyethylene terephthalate resin, polyethylene naphthalate resin, cycloolefin resin, polyimide resin, polycarbonate resin, etc. can be preferably used. In particular, as the material of the resin substrate that transmits visible light, polyamide, PET (polyethylene terephthalate), PEN (polyethylene naphthalate), COP (cycloolefin polymer), polyimide, polycarbonate, etc. can be more preferably used.
[0023] The thickness of the transparent substrate is not particularly limited, and can be arbitrarily selected according to the strength, capacitance, light transmittance, etc. required when used as a transparent conductive substrate. The thickness of the transparent substrate can be, for example, 10 μm or more and 200 μm or less. In particular, when used for touch panel applications, the thickness of the transparent substrate is preferably 20 μm or more and 120 μm or less, and more preferably 20 μm or more and 100 μm or less. In the case of use in touch panel applications, for example, in applications where a thin overall display is particularly required, the thickness of the transparent substrate is preferably 20 μm or more and 50 μm or less.
[0024] The total light transmittance of the transparent substrate is preferably high, and for example, the total light transmittance is preferably 30% or more, and more preferably 60% or more. When the total light transmittance of the transparent substrate is within the above range, for example, when the transparent substrate is used for a touch panel, the visibility of the display can be sufficiently ensured.
[0025] The total light transmittance of the transparent substrate can be evaluated by the method specified in JIS K 7361-1.
[0026] Next, the laminate will be described.
[0027] In the method for producing a transparent conductive substrate of the present embodiment, a laminate substrate having a transparent base material and a laminate disposed on at least one surface of the transparent base material is patterned to produce a transparent conductive substrate having a desired wiring pattern.
[0028] As described above, the laminate may have a structure in which a first blackened layer containing nickel and copper and a conductive layer containing copper are laminated in this order from the transparent substrate side. Note that, as described later, the laminate may further have a second blackened layer containing nickel and copper on the surface of the conductive layer opposite to the surface facing the first blackened layer.
[0029] The conductive layer only needs to contain copper (Cu), and other components are not particularly limited. They can be selected arbitrarily according to the electrical resistance value required for the transparent conductive substrate. The conductive layer is preferably a copper alloy containing, for example, Cu and at least one element selected from the group of elements Ni (nickel), Mo (molybdenum), Ta (tantalum), Ti (titanium), V (vanadium), Cr (chromium), Fe (iron), Mn (manganese), Co (cobalt), and W (tungsten), or a material containing Cu and at least one element selected from the above group of elements. The conductive layer can also be a copper layer made of copper.
[0030] Although the method for forming the conductive layer on the transparent substrate is not particularly limited, it is preferable that no adhesive is disposed between the conductive layer and the first blackening layer so as not to reduce the light transmittance, i.e., the conductive layer is preferably formed directly on the upper surface of the first blackening layer.
[0031] Since the conductive layer is formed directly on the upper surface of the first blackening layer, the conductive layer preferably has a conductive thin film layer, or may have a conductive thin film layer and a conductive plating layer.
[0032] For example, a conductive thin film layer can be formed on the first blackened layer by dry plating, and the conductive thin film layer can be used as the conductive layer. This allows the conductive layer to be formed directly on the first blackened layer without using an adhesive. Note that, for example, sputtering, vapor deposition, ion plating, etc. can be preferably used as the dry plating method.
[0033] Furthermore, when the thickness of the conductive layer is to be increased, the conductive thin film layer can be used as a power supply layer to form a conductive plating layer by, for example, electroplating, which is a type of wet plating method, thereby forming a conductive layer having a conductive thin film layer and a conductive plating layer. By having a conductive thin film layer and a conductive plating layer, the conductive layer can also be formed directly on the first blackened layer without using an adhesive.
[0034] The thickness of the conductive layer is not particularly limited, and can be arbitrarily selected depending on the magnitude of the current supplied to the wiring, the wiring width, etc., when the conductive layer is patterned and used as wiring.
[0035] However, if the conductive layer is thick, side etching may occur easily because etching of the conductive layer for patterning the laminate takes time, which may cause problems such as difficulty in forming fine lines, etc. For this reason, the thickness of the conductive layer is preferably 5 μm or less, and more preferably 3 μm or less.
[0036] Furthermore, particularly from the viewpoint of reducing the resistance value of the transparent conductive substrate and enabling a sufficient current supply, the conductive layer preferably has a thickness of 50 nm or more, more preferably 60 nm or more, and even more preferably 150 nm or more.
[0037] When the conductive layer has a conductive thin film layer and a conductive plating layer as described above, it is preferable that the sum of the thickness of the conductive thin film layer and the thickness of the conductive plating layer is within the above range.
[0038] In either case where the conductive layer is composed of a conductive thin film layer or a conductive thin film layer and a conductive plating layer, the thickness of the conductive thin film layer is not particularly limited, but is preferably, for example, 50 nm or more and 500 nm or less.
[0039] The conductive layer can be patterned into a shape corresponding to a desired wiring pattern to form a conductive wiring layer, which is wiring. The pattern shape of the conductive wiring layer is not particularly limited, and can be a shape corresponding to the wiring pattern required for the transparent conductive substrate.
[0040] The conductive wiring layer can be formed, for example, by patterning the conductive layer as described above. Therefore, when the conductive layer is composed of a conductive thin film layer, the conductive wiring layer can have a patterned conductive thin film layer. Also, when the conductive layer has a conductive thin film layer and a conductive plating layer, the conductive wiring layer can have a patterned conductive thin film layer and a patterned conductive plating layer.
[0041] The conductive layer can have a lower electrical resistance than ITO, which has traditionally been used as a material for the conductive layers of transparent conductive substrates. Therefore, by providing wiring patterned from the conductive layer, the electrical resistance of the transparent conductive substrate can be reduced.
[0042] Next, the first blackening layer will be described.
[0043] When a conductive layer or a conductive wiring layer is directly formed on a transparent substrate, the adhesion between the transparent substrate and the conductive layer or the conductive wiring layer may not be sufficient. Therefore, when a conductive layer or a conductive wiring layer is directly disposed on the upper surface of the transparent substrate, the conductive layer or the conductive wiring layer may peel off from the transparent substrate during the manufacturing process or during use. In addition, it may be required to suppress the reflection of light on the surface of the conductive layer or the conductive wiring layer due to light incident from the transparent substrate side.
[0044] Therefore, the laminate substrate used in the manufacturing method of the transparent conductive substrate of this embodiment can have a first blackening layer between the conductive layer and the transparent substrate in order to increase adhesion between the transparent substrate and the conductive layer and to suppress reflection on the conductive layer surface of light incident from the transparent substrate side.
[0045] The first blackening layer may contain nickel and copper, and other components are not particularly limited, but as described above, in order to suppress the reflection of light on the conductive layer surface, it is preferable that the first blackening layer has a color suitable for suppressing such reflection of light. For this reason, the first blackening layer preferably contains nickel, copper, and nickel oxide. The first blackening layer may further contain copper oxide. The nickel oxide and copper oxide may exist as a composite metal oxide, such as a metal oxide containing nickel and copper.
[0046] The first blackening layer may be composed of, for example, the above-mentioned nickel, copper, nickel oxide, and copper oxide. The first blackening layer may further contain an optional component. As the optional component, it may contain, for example, hydroxides of one or more metals selected from nickel and copper.
[0047] The method for forming the first blackening layer is not particularly limited, but it is preferable to form the layer by a dry plating method. As the dry plating method, for example, a sputtering method, an ion plating method, a vapor deposition method, etc. can be preferably used. When forming the first blackening layer by a dry method, it is more preferable to use a sputtering method because the film thickness can be easily controlled. As described above, the first blackening layer can also contain oxides such as nickel oxide. For this reason, oxygen can be added to the atmosphere when forming the first blackening layer, and in this case, a reactive sputtering method can be more preferably used.
[0048] By adding oxygen to the atmosphere during the deposition of the first blackening layer, oxygen can be added to the first blackening layer, and an oxide can be generated.
[0049] When forming the first blackening layer, oxygen is preferably added to, for example, an inert gas to be used as the atmospheric gas during dry plating. The inert gas is not particularly limited, but for example, argon can be preferably used.
[0050] By forming the first blackening layer by the dry plating method as described above, it is possible to improve the adhesion between the transparent substrate and the first blackening layer. In addition, since the first blackening layer can contain, for example, a metal as a main component, it also has high adhesion to the conductive layer. Therefore, by disposing the first blackening layer between the transparent substrate and the conductive layer, it is possible to suppress peeling of the conductive layer and the conductive wiring layer formed from the conductive layer.
[0051] The thickness of the first blackening layer is not particularly limited, but is preferably, for example, 3 nm to 50 nm, more preferably 3 nm to 35 nm, and even more preferably 3 nm to 33 nm.
[0052] It is preferable that the thickness of the first blackening layer is 3 nm or more, since this can particularly suppress the reflection of light on the surface of the conductive layer.
[0053] However, if the first blackening layer is made thicker than necessary, the time required for film formation and the time required for etching when patterning the first blackening layer will be longer, leading to increased costs. For this reason, the thickness of the first blackening layer is preferably 50 nm or less, more preferably 35 nm or less, and even more preferably 33 nm or less, as described above.
[0054] Next, the second blackening layer will be described.
[0055] The laminate of the laminate substrate provided in the method for producing a transparent conductive substrate of this embodiment may further have a second blackened layer containing nickel and copper on the surface of the conductive layer opposite to the surface facing the first blackened layer.
[0056] By providing the second blackening layer, it is possible to suppress light reflection on the surface of the conductive layer where the first blackening layer is not provided, which is preferable.
[0057] The second blackening layer may contain nickel and copper, and other components are not particularly limited, but as described above, in order to suppress the reflection of light on the conductive layer surface, it is preferable that the second blackening layer has a color suitable for suppressing such reflection of light. For this reason, the second blackening layer preferably contains nickel, copper, and nickel oxide. The second blackening layer may further contain copper oxide. The nickel oxide and copper oxide may exist as a composite metal oxide, such as a metal oxide containing nickel and copper.
[0058] The second blackening layer may be composed of, for example, the above-mentioned nickel, copper, nickel oxide, and copper oxide. The second blackening layer may further contain an optional component. As the optional component, it may contain, for example, hydroxides of one or more metals selected from nickel and copper.
[0059] The first blackened layer and the second blackened layer may have the same composition, or may have different compositions. As already explained, both the first blackened layer and the second blackened layer may contain nickel and copper. In addition, the first blackened layer and the second blackened layer may further contain nickel oxide, copper oxide, and one or more hydroxides selected from nickel and copper. Therefore, the first blackened layer and the second blackened layer may contain the same components, and the content ratios of the components may be the same or different. In addition, the first blackened layer and the second blackened layer may contain different components.
[0060] The method for forming the second blackening layer is not particularly limited, and any method can be selected as long as it can form the second blackening layer so as to contain nickel and copper. However, it is preferable to form the second blackening layer directly on the upper surface of another member such as a conductive layer without using an adhesive.
[0061] The second blackening layer can be formed, for example, by wet plating or dry plating. In the case of wet plating, for example, electroplating can be used, and in the case of dry plating, for example, sputtering, ion plating, vapor deposition, etc. can be used. In the case of dry plating, it is preferable to use sputtering, since it is particularly easy to control the film thickness.
[0062] As described above, the second blackening layer may also contain oxides such as nickel oxide, etc. Therefore, when the second blackening layer is formed by a dry plating method, oxygen may be added to the atmosphere during film formation, and in this case, a reactive sputtering method may be more preferably used.
[0063] By adding oxygen to the atmosphere when the second blackened layer is formed by dry plating, oxygen can be added to the second blackened layer to generate an oxide.
[0064] When forming the second blackening layer, oxygen is preferably added to, for example, an inert gas to be used as the atmospheric gas during dry plating. The inert gas is not particularly limited, but for example, argon can be preferably used.
[0065] The thickness of the second blackening layer is not particularly limited, and can be arbitrarily selected depending on the degree of suppression of light reflection required for the transparent conductive substrate.
[0066] The thickness of the second blackening layer is preferably, for example, 15 nm or more, and more preferably 20 nm or more, and is preferably 15 nm or more because the thickness of the second blackening layer is 15 nm or more, which can more reliably suppress light reflection on the surface of the conductive layer.
[0067] Although there is no particular upper limit to the thickness of the second blackening layer, if it is made thicker than necessary, the time required for etching in the patterning step will be longer, leading to increased costs. For this reason, the thickness of the second blackening layer is preferably 70 nm or less, and more preferably 50 nm or less.
[0068] Here, the configuration of the laminate substrate will be described with reference to Figures 1A and 1B. Figures 1A and 1B each show a schematic cross-sectional view of a transparent base material and a plane parallel to the lamination direction of the laminate.
[0069] 1A, the laminate substrate 10A can have a transparent base material 11 and a laminate 121 disposed on one surface 11a of the transparent base material 11. The laminate 121 can have a first blackening layer 121A and a conductive layer 121B in this order from the transparent base material 11 side.
[0070] 1B, the laminate substrate 10B can have a transparent base material 11 and a laminate 122 disposed on one surface 11a of the transparent base material 11. In the case of the laminate substrate 10B shown in FIG. 1B, the laminate 122 can have a structure in which a first blackening layer 122A, a conductive layer 122B, and a second blackening layer 122C are laminated in this order from the transparent base material 11 side.
[0071] 1A and 1B show an example of a laminate substrate in which a laminate is disposed only on one surface 11a of the transparent substrate 11, but the present invention is not limited to this embodiment, and a laminate substrate in which a laminate is disposed on the other surface 11b of the transparent substrate 11 may also be used. When a laminate is disposed on the other surface 11b of the transparent substrate 11, the laminates disposed above and below the transparent substrate 11 may be configured symmetrically or may be configured to have different configurations. For example, in the laminate substrate 10A shown in FIG. 1A, a laminate having a structure in which a first blackening layer 122A, a conductive layer 122B, and a second blackening layer 122C are laminated in this order from the transparent substrate 11 side may be disposed on the other surface 11b, similar to the laminate 122 shown in FIG. 1B.
[0072] Next, an example of the configuration of each process and step of the method for producing a transparent conductive substrate according to the present embodiment will be described with reference to the drawings. Note that in the attached drawings, the same members are given the same numbers, and some of the descriptions will be omitted.
[0073] The method for producing a transparent conductive substrate of this embodiment can include a patterning step of patterning a laminate substrate including a transparent substrate and a laminate disposed on at least one surface of the transparent substrate.
[0074] 2A to 2D show an example of a patterning process performed using the laminate substrate 10A shown in Fig. 1A. Fig. 2A to 2D show schematic cross-sectional views of the laminate substrate 10A in a plane parallel to the lamination direction of the transparent base material 11 and the laminate 121.
[0075] When carrying out the patterning step of the method for producing a transparent conductive substrate of this embodiment, a resist pattern 21 can be arranged in advance on a surface 121b of the laminate 121 of the laminate substrate 10A opposite to a surface 121a facing the transparent base material 11. The resist pattern 21 can have an opening 21A having a shape corresponding to a portion of the laminate 121 to be removed in the patterning step.
[0076] The patterning process may include a conductive layer etching step of etching the conductive layer with a first etchant capable of dissolving copper.
[0077] By carrying out the conductive layer etching step, the conductive layer 121B of the laminate 121 can be patterned as shown in Fig. 2B to form the conductive wiring layer 22, which is a wiring. At this time, the first blackened layer 121A is hardly etched, so that it can maintain the same shape as before carrying out the conductive layer etching step, as shown in Fig. 2B.
[0078] The first etching solution is not particularly limited as long as it can dissolve copper, but for example, an aqueous solution containing one selected from sulfuric acid, hydrogen peroxide, hydrochloric acid, cupric chloride, and ferric chloride, or a mixed aqueous solution containing two or more selected from the above sulfuric acid, etc. is more preferably used. The content of each component in the etching solution is not particularly limited. However, it is preferable to adjust the concentration of each component in the first etching solution so that the conductive layer can be selectively etched.
[0079] The etching solution can be used at room temperature, but can also be heated to enhance reactivity, for example, at 30° C. or higher and 50° C. or lower.
[0080] Next, a first blackening layer etching step can be performed in which the first blackening layer is etched with a second etching solution containing chloride ions and water.
[0081] By carrying out the first blackening layer etching step, the first blackening layer 121A of the laminate 121, which remained unpatterned after the conductive layer etching step as shown in FIG. 2C, can be patterned to form the patterned first blackening layer, that is, the first blackening wiring layer 23.
[0082] Furthermore, in the first blackening layer etching step, by using a second etching solution containing chloride ions and water, the first blackening layer containing nickel and copper can be patterned into a desired shape while suppressing the generation of residues, and the occurrence of side etching of the conductive wiring layer 22 can be suppressed.
[0083] The second etching solution may contain chloride ions and water as described above, and there are no particular limitations on the concentration of each component and other components. However, in order to sufficiently increase the reactivity with the first blackened layer, the concentration of chloride ions in the second etching solution is preferably 10 mass% or more in terms of hydrochloric acid. The concentration of chloride ions in terms of hydrochloric acid means a concentration calculated on the assumption that all chloride ions contained in the second etching solution are contained in the form of hydrochloric acid (HCl).
[0084] Moreover, the second etching liquid preferably contains hydrochloric acid and water. When the second etching liquid contains hydrochloric acid and water, the concentration of hydrochloric acid is not particularly limited, but is preferably 10 mass % or more and 37 mass % or less.
[0085] This is because the reactivity with the first blackened layer can be sufficiently increased by setting the concentration of hydrochloric acid to 10% by mass or more, and because the concentration of hydrochloric acid that is generally available is about 37% by mass or less, and from the viewpoint of cost, etc., it is preferable that the concentration be 37% by mass or less.
[0086] The second etching solution may also contain, for example, one or more selected from iron chloride and copper chloride.
[0087] However, if the iron ion concentration or copper ion concentration in the second etching liquid becomes too high, there is a risk of eroding the conductive layer or the conductive wiring layer formed by patterning the conductive layer. For this reason, the iron ion concentration in the second etching liquid is preferably 0.2 mass% or less. Also, the copper ion concentration in the second etching liquid is preferably 0.4 mass% or less. Note that the second etching liquid may be configured not to contain iron ions or copper ions, so that the iron ion concentration can be 0 or more. Also, the copper ion concentration can be 0 or more.
[0088] From the above, the second etching liquid contains hydrochloric acid and water, and the hydrochloric acid concentration is 10 mass % or more and 37 mass % or less, and the iron ion concentration can be 0.2 mass % or less.
[0089] The second etching liquid may contain, for example, hydrochloric acid and water, with a hydrochloric acid concentration of 10 mass % or more and 37 mass % or less, and a copper ion concentration of 0.4 mass % or less.
[0090] After the patterning process, as shown in FIG. 2D, the resist pattern 21 can be peeled off and removed to obtain a transparent conductive substrate having a conductive wiring layer 22 formed by patterning the conductive layer and the blackened layer, and a first blackened wiring layer 23 which is a patterned first blackened layer.
[0091] Any method can be used to peel and remove the resist pattern 21 depending on the type of resist used. For example, the resist pattern can be immersed in an aqueous sodium hydroxide solution to swell, peel and remove it.
[0092] Between the conductive layer etching step and the first blackening layer etching step in the patterning process, or after the first blackening layer etching step, the laminate substrate undergoing the patterning process may be washed with water, for example. By washing with water after each step of the patterning process in this way, it is possible to prevent the etching solution adhering to the laminate substrate from being carried over to the subsequent process. After the resist pattern is peeled off, washing with water, drying, etc. can be performed as necessary. Similarly, in the case of other configuration examples of the patterning process described later, the laminate substrate undergoing the patterning process may be washed with water between each step or after each step.
[0093] The laminate substrate used in the method for producing a transparent conductive substrate of the present embodiment may also have a second blackening layer as described above. One configuration example of the method for producing a transparent conductive substrate of the present embodiment in such a case will be described below with reference to Figures 3A to 3E.
[0094] As described using FIG. 1B, the laminate 122 of the laminate substrate 10B may further have a second blackened layer 122C containing nickel and copper on the surface opposite to the surface facing the first blackened layer 122A of the conductive layer 122B.
[0095] 3A, a resist pattern 31 can be arranged in advance on a surface 122b of the laminate 122 of the laminate substrate 10B opposite to a surface 122a facing the transparent base material 11. The resist pattern 31 can have an opening 31A having a shape corresponding to a portion of the laminate 122 to be removed in the patterning step.
[0096] In addition, the patterning process may further include, before the conductive layer etching step, a second blackening layer etching step of etching the second blackening layer 122C with a second etching solution, as shown in FIG. 3B.
[0097] The second etching solution has already been described, so a description thereof will be omitted here.
[0098] By carrying out the second blackening layer etching step, as shown in Fig. 3B, the second blackening layer 122C of the laminate 122 can be patterned to form the patterned second blackening layer, which is the second blackening wiring layer 32. The conductive layer 122B is hardly etched by the second etching solution, so that it can maintain substantially the same shape as before the second blackening layer etching step, as shown in Fig. 3B.
[0099] Thereafter, in the same manner as in the above-described configuration example, a conductive layer etching step can be performed in which the conductive layer 122B is etched with a first etching solution capable of dissolving copper, whereby the conductive layer 122B can be patterned into the conductive wiring layer 33 as shown in FIG.
[0100] Next, a first blackening layer etching step can be performed in which the first blackening layer 122A is etched with a second etching solution containing chloride ions and water, thereby forming a first blackening wiring layer 34, which is a patterned first blackening layer, as shown in FIG.
[0101] The conductive layer etching step and the first blackening layer etching step have already been described, and therefore will not be described here.
[0102] After the patterning process, as shown in FIG. 3E, the resist pattern 31 is peeled off and removed to obtain a transparent conductive substrate having the second blackened wiring layer 32, the conductive wiring layer 33, and the first blackened wiring layer 34, in which the second blackened layer 122C, the conductive layer 122B, and the first blackened layer 122A are patterned.
[0103] Another configuration example of the method for producing a transparent conductive substrate of this embodiment will be described below with reference to Figs. 4A to 4D, in which the laminate of the laminate substrate used in the method for producing a transparent conductive substrate of this embodiment further has a second blackened layer containing nickel and copper on the surface of the conductive layer opposite to the surface facing the first blackened layer.
[0104] 4A, a resist pattern 41 can be arranged in advance on a surface 122b of the laminate 122 of the laminate substrate 10B opposite to a surface 122a facing the transparent base material 11. The resist pattern 41 can have an opening 41A having a shape corresponding to a portion of the laminate 122 to be removed in the patterning step.
[0105] Then, in the conductive layer etching step of the patterning process, as shown in FIG. 4B, the conductive layer 122B and the second blackening layer 122C can be etched by a first etching solution.
[0106] As described above, the first etching solution can etch the conductive layer 122B, and has low reactivity with the second blackened layer 122C. However, since the second blackened layer 122C is disposed on the conductive layer 122B, the second blackened layer 122C can be etched by etching the conductive layer 122B.
[0107] Therefore, by carrying out the conductive layer etching step, the second blackened wiring layer 42 and the conductive wiring layer 43 can be formed.
[0108] The first etching solution has already been described, so a description thereof will be omitted here.
[0109] Thereafter, in the same manner as in the case of the above-described configuration example, a first blackening layer etching step can be performed in which the first blackening layer 122A is etched with a second etching solution containing chloride ions and water, thereby forming a first blackening wiring layer 44 as shown in FIG.
[0110] The first blackening layer etching step has already been described, so a description thereof will be omitted here.
[0111] After the patterning process, as shown in FIG. 4D, the resist pattern 41 is peeled off and removed to obtain a transparent conductive substrate having the second blackened wiring layer 42, the conductive wiring layer 43, and the first blackened wiring layer 44, in which the second blackened layer 122C, the conductive layer 122B, and the first blackened layer 122A are patterned.
[0112] Although an example of performing the patterning step using a laminate substrate in which a laminate is disposed only on one surface of the transparent base material 11 has been shown, the present invention is not limited to such an embodiment. For example, the patterning step can be performed using a laminate substrate in which a laminate is disposed on one surface of the transparent base material and on the other surface located opposite to the one surface. The patterning step can be performed simultaneously for the laminate disposed on one surface and the laminate disposed on the other surface, or the patterning step can be performed separately for each of them.
[0113] The pattern formed in the patterning step of the transparent conductive substrate of this embodiment is not particularly limited, and can be arbitrarily selected according to the application. For example, when used for a touch panel, a transparent conductive substrate having mesh-shaped (lattice-shaped) wiring may be required. For this reason, for example, the conductive layer can be patterned to become a lattice-shaped conductive wiring layer. In addition, since the first blackening layer and the second blackening layer are provided to suppress the reflection of light on the surface of the conductive layer, it is preferable to pattern these layers so that the cross-sectional shape on a plane parallel to the surface on which the laminate of the transparent base material is arranged is the same shape as the conductive wiring layer.
[0114] A configuration example of a transparent conductive substrate having mesh-like wiring will be described. A transparent conductive substrate having mesh-like wiring can be formed using one transparent conductive substrate, but a transparent conductive substrate having mesh-like wiring can also be formed using a combination of two transparent conductive substrates.
[0115] Fig. 5 shows a top view of a transparent conductive substrate having mesh-like wiring, and Figs. 6A and 6B show examples of cross-sectional views taken along line AA' in Fig. 5. The top view is a view seen from above in a direction perpendicular to the surface on which the laminate of transparent base material 11 is arranged. Although the first and second blackened wiring layers are omitted in Fig. 5, the first and second blackened wiring layers can have the same cross-sectional shape as the adjacent conductive wiring layers 51A and 51B in a plane parallel to the surface on which the conductive wiring layers 51A and the like of transparent base material 11 are arranged.
[0116] In the transparent conductive substrate 50 shown in FIG. 5, a grid-like wiring is formed by linear conductive wiring layers 51A parallel to the Y-axis direction and linear conductive wiring layers 51B parallel to the X-axis direction.
[0117] As shown in Fig. 6A, a configuration can be adopted in which a conductive wiring layer 51A is disposed on one surface 11a of the transparent base material 11, and a conductive wiring layer 51B is disposed on the other surface 11b. In this case, as shown in Fig. 6A, first blackened wiring layers 52A and 52B can be disposed on the transparent base material 11 side of the conductive wiring layers 51A and 51B. Also, a configuration can be adopted in which second blackened wiring layers 53A and 53B are disposed on the surface of the conductive wiring layers 51A and 51B opposite to the transparent base material 11 side. Note that a structure without the second blackened wiring layers 53A and 53B is also acceptable.
[0118] The transparent conductive substrate having the structure shown in FIG. 5 and FIG. 6A can be manufactured, for example, by the following procedure. First, two laminate substrates each having a laminate disposed on one surface of a transparent base material are patterned to have a plurality of linear patterns parallel to each other by the patterning process described above. Then, the two transparent conductive substrates are aligned in the direction so that the plurality of linear wirings of the two transparent conductive substrates are in a mesh shape, and the other surfaces of the transparent base material on which the laminate is not disposed are bonded together to manufacture the substrate. In this case, the transparent base material 11 in FIG. 6A is configured by bonding two transparent base materials together.
[0119] The transparent conductive substrate having the structure shown in Fig. 5 and Fig. 6A can also be manufactured by the following procedure. First, a laminate substrate is prepared in which a laminate is disposed on one surface of a transparent base material and on the other surface opposite to the one surface. Then, the laminate disposed on both surfaces of the transparent base material is patterned in a patterning process so that the conductive wiring layer, which is the wiring of the laminate, has the same configuration as Fig. 5 and Fig. 6A.
[0120] 5 and 6B, the conductive wiring layer 51A may be disposed on the transparent substrate 11A, and the conductive wiring layer 51B may be disposed between the transparent substrate 11A and the transparent substrate 11B. In this case, the first blackened wiring layers 52A and 52B may be disposed on the transparent substrate 11A and 11B side of the conductive wiring layers 51A and 51B. In addition, the second blackened wiring layers 53A and 53B may be disposed on the surface of the conductive wiring layers 51A and 51B opposite to the transparent substrate 11A and 11B side. In this case, the second blackened wiring layers 53A and 53B may not be disposed.
[0121] The transparent conductive substrate having the structure shown in FIG. 5 and FIG. 6B can be manufactured, for example, by the following procedure. First, two laminate substrates each having a laminate disposed on one surface of a transparent base material are patterned into a plurality of parallel linear patterns by the patterning process described above. Then, the two transparent conductive substrates are aligned in the direction so that the plurality of linear wirings are in a mesh shape, and the other surface of one transparent conductive substrate on which the laminate of the transparent base material of the transparent conductive substrate is not disposed is bonded to the exposed surface of the patterned laminate of the other transparent conductive substrate, thereby manufacturing the substrate.
[0122] 5, 6A, and 6B show examples of linear wiring, i.e., mesh-shaped wiring (wiring pattern) formed by combining conductive wiring layers, but the present invention is not limited to such a form, and the wiring constituting the wiring pattern can be of any shape. For example, the shape of the conductive wiring layers constituting the mesh-shaped wiring pattern can be various shapes such as jaggedly bent lines (zigzag straight lines) so that moire (interference fringes) does not occur with the display image.
[0123] The method for producing a transparent conductive substrate of this embodiment may include any step other than the above-mentioned patterning step.
[0124] For example, a resist disposing step may be further included, prior to the patterning step, of disposing a resist on an exposed surface of the laminate, which is the surface opposite to the surface facing the transparent substrate.
[0125] The resist placement process may further include the following steps:
[0126] A photosensitive resist layer forming step of forming a photosensitive resist layer on the exposed surface. A resist pattern forming step in which the photosensitive resist layer is exposed to ultraviolet light according to a resist pattern to be formed, and the unexposed areas are developed to form a resist pattern.
[0127] In the resist placement step, the resist patterns 21, 31, and 41 shown in FIG. 2A, FIG. 3A, and FIG. 4A can be formed.
[0128] 2A, first, a photosensitive resist layer can be formed on surface 121b opposite to surface 121a of laminate 121 facing transparent base material 11. The method of forming the photosensitive resist layer depends on the type of resist used, but examples include a method of applying the photosensitive resist layer onto surface 121b of laminate 121 on which the resist is to be placed, and a method of attaching the photosensitive resist layer by a lamination method or the like.
[0129] Then, using a mask or the like, the resist is exposed to ultraviolet light according to the resist pattern to be formed, and the unexposed portions are developed and removed, for example, to form the resist pattern.
[0130] The method for developing the photosensitive resist layer is not particularly limited, but may be a method of immersing the layer in a developer such as an aqueous sodium carbonate solution.
[0131] The method for producing the transparent conductive substrate of this embodiment may also include, for example, a laminate substrate production step.
[0132] The laminate substrate manufacturing process can further include, for example, the following steps.
[0133] A first blackening layer forming step of forming a first blackening layer on at least one surface of the transparent substrate. A conductive layer forming step of forming a conductive layer on the first blackening layer. Furthermore, if necessary, the method may further include a second blackening layer forming step of forming a second blackening layer on the conductive layer.
[0134] Specific examples of methods for forming the first blackened layer, the conductive layer, and the second blackened layer have already been described, and therefore will not be described here.
[0135] Furthermore, a lamination step may be included in which a plurality of transparent conductive substrates after the patterning step are laminated together to form, for example, mesh-like wiring, as described above.
[0136] According to the method for producing a transparent conductive substrate of the present embodiment described above, the first blackened layer and the conductive layer in contact with the transparent base material are etched with different etching solutions, which makes it possible to prevent the first blackened layer from remaining on the transparent base material and to prevent the side etching of the conductive layer from becoming large.
[0137] Therefore, according to the method for producing a transparent conductive substrate of this embodiment, the blackening layer can be patterned into a desired shape. [Transparent conductive substrate] Next, a configuration example of the transparent conductive substrate of this embodiment will be described.
[0138] The transparent conductive substrate of this embodiment can be manufactured by, for example, the above-mentioned method for manufacturing a transparent conductive substrate, and therefore some of the matters already described will not be described again.
[0139] The first blackened wiring layer, conductive wiring layer, and second blackened wiring layer described below can be formed by patterning the first blackened layer, conductive layer, and second blackened layer, respectively, as described above. Therefore, the first blackened wiring layer, conductive wiring layer, and second blackened wiring layer can have the same configuration as the first blackened layer, conductive layer, and second blackened layer described above in the manufacturing method for the transparent conductive substrate, respectively, except for being patterned.
[0140] The transparent conductive substrate of the present embodiment can have a transparent base material and thin metal wires disposed on at least one surface of the transparent base material. The thin metal wires may be a laminate in which a first blackened wiring layer containing nickel and copper and a conductive wiring layer containing copper are laminated in that order from the transparent base material side. Furthermore, when viewed from a direction perpendicular to one surface of the transparent base material, the protruding width of the first blackened wiring layer protruding from the conductive wiring layer can be set to 0.5 μm or less.
[0141] First, the transparent conductive substrate of this embodiment will be described with reference to Figures 7A and 7B. Figure 7A is a schematic cross-sectional view of the transparent conductive substrate of this embodiment taken along a plane parallel to the lamination direction of the transparent base material and thin metal wires.
[0142] As shown in FIG. 7A, the transparent conductive substrate 70 of this embodiment can have a structure in which a first blackened wiring layer 712 and a thin metal wire 71 having a conductive wiring layer 711 are arranged on at least one surface 11a of a transparent base material 11.
[0143] FIG. 7B shows an enlarged view of the area B surrounded by a dotted line when the transparent conductive substrate 70 shown in FIG. 7A is viewed from a direction perpendicular to one surface 11a of the transparent base material 11, i.e., when the transparent conductive substrate is viewed along the block arrow A in the figure.
[0144] As described above in the method for producing a transparent conductive substrate, the first blackened layer, etc., can be patterned to form the thin metal wires 71 in which the first blackened wiring layer 712 and the conductive wiring layer 711 are patterned on the transparent base material 11. However, in the process of patterning the first blackened layer, etc., the first blackened layer may remain partially dissolved, causing the first blackened wiring layer 712 to protrude beyond the conductive wiring layer 711. In the transparent conductive substrate of this embodiment, the protruding width L of the first blackened wiring layer 712 is preferably 0.5 μm or less.
[0145] Since it is preferable that the protruding width L of the first blackened wiring layer 712 is zero, the protruding width L of the first blackened wiring layer 712 can be set to zero or more.
[0146] The method for setting the protrusion width L of the first blackened wiring layer 712 in the above range is not particularly limited, but for example, the above range can be achieved by using the above-mentioned manufacturing method for the transparent conductive substrate.
[0147] 7A and 7B show an example in which the thin metal wire is composed of the first blackened wiring layer 712 and the conductive wiring layer 711, but is not limited to such an example. For example, the thin metal wire may further have a second blackened wiring layer containing nickel and copper on the surface of the conductive wiring layer 711 opposite to the surface facing the first blackened wiring layer 712.
[0148] In addition, in FIG. 7A, an example in which the thin metal wire is disposed only on one surface 11a of the transparent substrate 11 is shown, but the present invention is not limited to this form. As described with reference to FIG. 6A and the like, the thin metal wire can also be disposed on the other surface 11b of the transparent substrate 11. In this case, the thin metal wire disposed on one surface 11a of the transparent substrate 11 and the thin metal wire disposed on the other surface 11b may have different layer configurations. For example, a thin metal wire having a first blackened wiring layer and a conductive wiring layer can be disposed on one surface 11a, and a thin metal wire having a first blackened wiring layer, a conductive wiring layer, and a second blackened wiring layer can be disposed on the other surface 11b. However, in any of the thin metal wires, it is preferable that the protruding width of the first blackened wiring layer contained therein satisfies the above-mentioned range.
[0149] In addition, when a thin metal wire is arranged on the other surface, the protruding width of the first blackened wiring layer protruding from the conductive wiring layer of the thin metal wire on the other surface side can be measured by viewing from the other surface side of the transparent substrate so that the protrusion can be confirmed. Since the transparent substrate usually has one surface and the other surface parallel to each other, when measuring the protruding width of the first blackened wiring layer on the other surface side, viewing from a direction perpendicular to one surface of the transparent substrate can also be rephrased as viewing from a direction perpendicular to the other surface of the transparent substrate. In addition, when thin metal wires are arranged on one surface and the other surface of the transparent substrate in this way, the protruding width of the first blackened wiring layer means the protruding width from the conductive wiring layer located on the same side as the first blackened layer, i.e., the adjacent conductive wiring layer.
[0150] Furthermore, as described with reference to, for example, FIGS. 5, 6A, and 6B, a transparent conductive substrate having mesh-like wiring can be formed by combining a plurality of conductive wiring layers.
[0151] It is preferable that the cross-sectional shape of the first blackened wiring layer in a plane parallel to the surface of the transparent substrate on which the thin metal wires are provided is the same as that of the conductive wiring layer. Therefore, when the conductive wiring layers are combined to form a conductive substrate having mesh-shaped wiring, it is preferable that the first blackened wiring layer included in the transparent conductive substrate is also combined to form a mesh. When the second blackened wiring layer is provided on both surfaces of the transparent substrate, the same can be said for the second blackened wiring layer.
[0152] In the transparent conductive substrate of this embodiment, by providing a first blackened wiring layer on the surface of the conductive wiring layer, the adhesion between the transparent base material and the conductive wiring layer can be improved, and reflection on the surface of the conductive wiring layer facing the first blackened wiring layer can be suppressed. The degree of light reflection on the surface of the first blackened wiring layer is not particularly limited, but for example, it is preferable that the average reflectance of light having a wavelength of 400 nm or more and 700 nm or less of the first blackened wiring layer is 15% or less.
[0153] In addition, the average reflectance of the first blackened wiring layer for light having a wavelength of 400 nm or more and 700 nm or less is preferably close to the average reflectance of the light for the transparent substrate. Therefore, the lower limit of the average reflectance of the first blackened wiring layer for light having a wavelength of 400 nm or more and 700 nm or less can be selected according to the transparent substrate used, and is not particularly limited. For example, when a polyethylene terephthalate resin or the like is used as the transparent substrate, the average reflectance of the light having a wavelength of 400 nm or more and 700 nm or less is about 6%. Even if the average reflectance of the first blackened wiring layer for light having a wavelength of 400 nm or more and 700 nm or less is 0, the difference in the average reflectance of the light with the transparent substrate such as polyethylene terephthalate resin can be reduced to about 6%. Therefore, the average reflectance of the first blackened wiring layer for light having a wavelength of 400 nm or more and 700 nm or less can be, for example, 0 or more.
[0154] The light reflectance of the first blackened wiring layer can be measured by irradiating the first blackened wiring layer of the transparent conductive substrate with light. Specifically, for example, in the case of a transparent conductive substrate 70 shown in FIG. 7A, in which the first blackened wiring layer 712 and the conductive wiring layer 711 are laminated in this order on one surface 11a of the transparent substrate 11, light is irradiated to the surface 712a of the first blackened wiring layer 712 through the transparent substrate 11 so as to irradiate the first blackened wiring layer 712 with light, and the measurement can be performed. In the measurement, light having a wavelength of 400 nm or more and 700 nm or less is irradiated to the surface 712a of the first blackened wiring layer 712 of the transparent conductive substrate as described above at wavelength intervals of 1 nm, for example, and the average value of the measured values can be regarded as the average reflectance of the first blackened wiring with light having a wavelength of 400 nm or more and 700 nm or less.
[0155] As described above, the first blackened wiring layer is formed by patterning the first blackened layer. Therefore, the average reflectance of the first blackened layer to light having a wavelength of 400 nm or more and 700 nm or less may be measured and calculated in advance, and the average value may be used as the average reflectance of the first blackened wiring layer to light having a wavelength of 400 nm or more and 700 nm or less. EXAMPLES
[0156] The present invention will be described below with reference to specific examples and comparative examples, but it should be understood that the present invention is not limited to these examples. [Experimental Example 1] Transparent conductive substrates were manufactured as Experimental Examples 1-1 to 1-30. Experimental Examples 1-4 to 1-18 are working examples, and Experimental Examples 1-1 to 1-3 and Experimental Examples 1-19 to 1-30 are comparative examples.
[0157] First, a laminate substrate was prepared in which a first blackening layer, a conductive layer, and a second blackening layer were laminated in that order on one side of a transparent substrate, which was a polyethylene terephthalate resin (PET) film with a thickness of 50 μm, to be subjected to a patterning process. The total light transmittance of the transparent substrate was evaluated by the method specified in JIS K 7361-1 and was found to be 93%. The same transparent substrate was used in the other experimental examples described below.
[0158] The first blackening layer has a thickness of 0.03 μm and contains nickel, copper, nickel oxide, and copper oxide.
[0159] The conductive layer was a copper layer with a thickness of 0.5 μm. The conductive layer included a conductive thin film layer (copper thin film layer) formed by a sputtering method and a conductive plating layer (copper plating layer) formed by an electroplating method. The other experimental examples below were similarly configured.
[0160] The second blackening layer has a thickness of 0.05 μm and contains nickel, copper, oxides of nickel, and oxides of copper.
[0161] The first and second blackening layers were both formed by reactive sputtering in an atmosphere of argon gas with added oxygen, as in the other experimental examples described below.
[0162] The first blackening layer and the second blackening layer had the same composition in the same laminate substrate, and three types of laminate substrates were prepared with different reflectances on the surface of the first blackening layer ranging from 12% to 16%.
[0163] The light reflectance on the surface of the first blackened layer was measured using an ultraviolet-visible spectrophotometer (Shimadzu Corporation, model: UV-2550) equipped with a reflectance measuring unit.
[0164] The surface of the first blackening layer was irradiated with light having a wavelength of 400 nm or more and 700 nm or less at 1 nm intervals through the transparent base material of the laminate substrate produced, with an incident angle of 5° and a receiving angle of 5°, to measure the regular reflectance, and the average value was taken as the reflectance. In the other experimental examples described below, the reflectance was measured in the same manner. Hereinafter, the average reflectance of light having a wavelength of 400 nm or more and 700 nm or less on the surface of the first blackening layer is also simply referred to as the reflectance on the surface of the first blackening layer. In the tables, it may also be simply referred to as the reflectance.
[0165] Furthermore, the content ratio of metallic nickel and nickel oxide or nickel hydroxide among the nickel components contained in the first blackened layer and the second blackened layer when the light reflectance on the surface of the first blackened layer is 12% to 16% is shown in Table 1. The reflectance values of 12% and 16% shown in Table 1 are values calculated based on the analysis results of XPS (X-ray Photoelectron Spectroscopy) when the reflectance is 14%, taking into consideration the amount of oxygen supplied during film formation of the first blackened layer and the second blackened layer.
[0166] In Table 1, for example, when the reflectance is 12%, this means that in the first blackened layer and the second blackened layer, 50.5 mass% of the nickel component is present as metallic nickel, and 49.5 mass% is present as nickel oxide, and in some cases, further as nickel hydroxide.
[0167] [Table 1] The prepared laminate substrate was cut to an arbitrary size, and then a resist placement process was carried out. Specifically, a photosensitive resist (manufactured by Asahi Kasei Corporation, product name: AQ-1F59) was attached to the surface of the second blackened layer by lamination to form a photosensitive resist layer (photosensitive resist layer formation step). Then, the photosensitive resist layer was exposed to ultraviolet light, and the unexposed parts were developed to form a mesh-patterned resist pattern (resist pattern formation step). Note that the resist pattern had a distance between adjacent lines of 0.1 mm, and a line width (resist width) of 13 μm.
[0168] The laminate substrate having the resist pattern formed on the surface of the second blackening layer was subjected to the following patterning steps, in which the laminate substrate was washed with water between each step.
[0169] As a first etching solution, a ferric chloride solution with a concentration of 25 mass % and a temperature of 30° C. was prepared. The prepared laminate substrate was then immersed in the first etching solution for 10 seconds to etch the conductive layer and the second blackened layer (conductive layer etching step).
[0170] Next, as the second etching solution, hydrochloric acid aqueous solutions with concentrations of 5% by mass to 37% by mass, nitric acid aqueous solutions with concentrations of 10% by mass and 35% by mass, and sulfuric acid aqueous solutions with concentrations of 10% by mass and 30% by mass were prepared for each experimental example, as shown in Table 2. The second etching solutions were used at room temperature (25°C). The copper ion concentration and iron ion concentration of the second etching solutions were all zero.
[0171] Then, the laminate substrate after the conductive layer etching step was immersed in the second etching solution of each experimental example, and the time until the first blackened layer was dissolved and no residue was left on the film and it appeared transparent to the naked eye was measured. The evaluation results are shown in Table 2.
[0172] [Table 2] According to the results shown in Table 2, it was confirmed that the first blackened layer can be etched in less than 180 seconds by using an aqueous hydrochloric acid solution containing chloride ions and water and having a chloride ion concentration of 10 mass% or more calculated as hydrochloric acid as the second etching solution. In other words, it was confirmed that the generation of residues of the first blackened layer on the transparent substrate can be suppressed, and the first blackened layer, conductive layer, and second blackened layer can be patterned into a desired shape.
[0173] In addition, when the obtained transparent conductive substrate was observed by SEM (scanning electron microscope, manufactured by JEOL Ltd., model: JSM-6360LV), it was confirmed that in all of Experimental Examples 1-4 to 1-18, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less.
[0174] On the other hand, when an aqueous solution of nitric acid or sulfuric acid that does not contain chloride ions was used as the second etching solution, it was confirmed that the first blackened layer could not be completely etched even after 180 seconds, and a residue of the first blackened layer was left on the transparent substrate. [Experimental Example 2] As Experimental Examples 2-1 to 2-6, transparent conductive substrates were produced and the influence of the copper ion concentration in the second etching liquid was examined. All of Experimental Examples 2-1 to 2-6 are examples.
[0175] First, a laminate substrate was prepared for the patterning process, in which a first blackened layer, a conductive layer, and a second blackened layer were laminated in that order on one surface of a transparent substrate, which was a 50 μm-thick polyethylene terephthalate resin (PET) film.
[0176] The first blackening layer has a thickness of 0.03 μm and contains nickel, copper, nickel oxide, and copper oxide. As the conductive layer, a copper layer having a thickness of 0.5 μm and configured in the same manner as in Experimental Example 1 was used.
[0177] The second blackening layer has a thickness of 0.05 μm and contains nickel, copper, oxides of nickel, and oxides of copper.
[0178] The first and second blackening layers had the same composition, and a laminate substrate was prepared with a reflectance of 14% on the surface of the first blackening layer. The first and second blackening layers had the same composition as in Experimental Example 1-5.
[0179] The prepared laminate substrate was cut to an arbitrary size, and then a resist placement process was carried out. Specifically, a photosensitive resist (manufactured by Asahi Kasei Corporation, product name: AQ-1F59) was attached to the surface of the second blackened layer by lamination to form a photosensitive resist layer (photosensitive resist layer formation step). Then, the photosensitive resist layer was exposed to ultraviolet light, and the unexposed parts were developed to form a mesh-patterned resist pattern (resist pattern formation step). Note that the resist pattern had a distance between adjacent lines of 0.1 mm, and a line width (resist width) of 13 μm.
[0180] The laminate substrate having the resist pattern formed on the surface of the second blackening layer was subjected to the following patterning steps, with the laminate substrate being washed with water between each step.
[0181] As the second etching solution, an aqueous hydrochloric acid solution with a hydrochloric acid concentration of 25 mass % and a temperature of room temperature (25°C) was prepared. When preparing the second etching solution, cupric chloride was added to hydrochloric acid of the above concentration to adjust the copper ion concentration in the second etching solution for each experimental example as shown in Table 3. The iron ion concentration in the second etching solutions used in the present experimental examples was 0.
[0182] Then, the laminate substrate was immersed in a second etching solution for 30 seconds to etch the second blackened layer (second blackened layer etching step).
[0183] Next, as a first etching solution, a ferric chloride solution with a concentration of 25% by mass and a temperature of 30° C. was prepared. Then, the laminate substrate having completed the second blackening layer etching step was immersed in the first etching solution for 10 seconds to etch the conductive layer (conductive layer etching step).
[0184] Then, the first blackened layer was etched using the second etching solution used for etching the second blackened layer in each experimental example (first blackened layer etching step).
[0185] Thereafter, the substrate was immersed in an aqueous sodium hydroxide solution having a concentration of 5% by mass and a temperature of 40° C. for 60 seconds to swell, peel and remove the resist pattern, followed by washing with water and drying to obtain a transparent conductive substrate.
[0186] In all of the experimental examples, no residue of the first blackened layer was left on the transparent substrate.
[0187] The appearance of the conductive wiring layer of the obtained transparent conductive substrate was observed, and it was visually confirmed whether the conductive wiring layer was eroded. The evaluation results are shown in Table 3.
[0188] In Table 3, a rating of A was given when the wiring was formed normally, and a rating of B was given when thinning was observed in part of the wiring.
[0189] [Table 3] It was confirmed that the first blackened layer, the conductive layer, and the second blackened layer could be patterned into a desired shape in all of Experimental Examples 2-1 to 2-6. However, according to the results shown in Table 3, it was confirmed that when the copper ion concentration in the second etching solution was about 0.5 mass%, some thinning was observed in a part of the conductive wiring layer, which was the obtained wiring. From the above results, it was confirmed that the copper ion concentration in the second etching solution is preferably less than 0.5 mass%, and more preferably 0.4 mass% or less.
[0190] When the obtained transparent conductive substrates were observed by SEM, it was confirmed that in all of Experimental Examples 2-1 to 2-6, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less. [Experimental Example 3] As Experimental Examples 3-1 to 3-7, transparent conductive substrates were produced and the influence of the iron ion concentration in the second etching liquid was examined. All of Experimental Examples 3-1 to 3-7 are examples.
[0191] First, a laminate substrate was prepared for the patterning process, in which a first blackened layer, a conductive layer, and a second blackened layer were laminated in that order on one surface of a transparent substrate, which was a 50 μm-thick polyethylene terephthalate resin (PET) film.
[0192] The first blackening layer has a thickness of 0.03 μm and contains nickel, copper, nickel oxide, and copper oxide.
[0193] As the conductive layer, a copper layer having a thickness of 0.5 μm and configured in the same manner as in Experimental Example 1 was used.
[0194] The second blackening layer has a thickness of 0.05 μm and contains nickel, copper, oxides of nickel, and oxides of copper.
[0195] The first and second blackening layers had the same composition, and a laminate substrate was prepared with a reflectance of 14% on the surface of the first blackening layer. The first and second blackening layers had the same composition as in Experimental Example 1-5.
[0196] The prepared laminate substrate was cut to an arbitrary size, and then a resist placement process was carried out. Specifically, a photosensitive resist (manufactured by Asahi Kasei Corporation, product name: AQ-1F59) was attached to the surface of the second blackened layer by lamination to form a photosensitive resist layer (photosensitive resist layer formation step). Then, the photosensitive resist layer was exposed to ultraviolet light, and the unexposed parts were developed to form a mesh-patterned resist pattern (resist pattern formation step). The resist pattern had a distance between adjacent lines of 0.1 mm, and a line width (resist width) of 13 μm.
[0197] The laminate substrate having the resist pattern formed on the surface of the second blackening layer was subjected to the following patterning steps, with the laminate substrate being washed with water between each step.
[0198] As the second etching solution, an aqueous hydrochloric acid solution with a hydrochloric acid concentration of 25 mass% and a temperature of room temperature (25°C) was prepared. When preparing the second etching solution, ferric chloride was added to the hydrochloric acid of the above concentration to adjust the iron ion concentration in the second etching solution to a range of 0 to 0.3 mass% for each experimental example, as shown in Table 4. The copper ion concentration in the second etching solutions used in the present experimental examples was 0.
[0199] Then, the laminate substrate was immersed in a second etching solution for 30 seconds to etch the second blackened layer (second blackened layer etching step).
[0200] Next, as a first etching solution, a ferric chloride solution with a concentration of 25% by mass and a temperature of 30° C. was prepared. Then, the laminate substrate having completed the second blackening layer etching step was immersed in the first etching solution for 10 seconds to etch the conductive layer (conductive layer etching step).
[0201] Then, the first blackened layer was etched using the second etching solution used for etching the second blackened layer in each experimental example (first blackened layer etching step).
[0202] Thereafter, the substrate was immersed in an aqueous sodium hydroxide solution having a concentration of 5% by mass and a temperature of 40° C. for 60 seconds to swell, peel and remove the resist pattern, followed by washing with water and drying to obtain a transparent conductive substrate.
[0203] In all of the experimental examples, no residue of the first blackened layer was left on the transparent substrate.
[0204] The appearance of the conductive wiring layer of the obtained transparent conductive substrate was observed, and it was visually confirmed whether the conductive wiring layer was eroded. The evaluation results are shown in Table 4.
[0205] In Table 4, a rating of A was given when the wiring was formed normally, and a rating of B was given when thinning was observed in part of the wiring.
[0206] [Table 4] It was confirmed that the first blackened layer, the conductive layer, and the second blackened layer could be patterned into a desired shape in all of Experimental Examples 3-1 to 3-7. However, according to the results shown in Table 4, it was confirmed that when the iron ion concentration in the second etching solution was about 0.30 mass%, some thinning was observed in a part of the conductive wiring layer, which was the obtained wiring. From the above results, it was confirmed that the iron ion concentration in the second etching solution is preferably less than 0.30 mass%, and more preferably 0.20 mass% or less.
[0207] When the obtained transparent conductive substrates were observed by SEM, it was confirmed that in all of Experimental Examples 3-1 to 3-7, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less. [Experimental Example 4] Transparent conductive substrates were produced as Experimental Examples 4-1 and 4-2. Both Experimental Examples 4-1 and 4-2 are examples of the present invention.
[0208] First, a laminate substrate was prepared for the patterning process, in which a first blackened layer, a conductive layer, and a second blackened layer were laminated in that order on one surface of a transparent substrate, which was a 50 μm-thick polyethylene terephthalate resin (PET) film.
[0209] The first blackening layer has a thickness of 0.03 μm and contains nickel, copper, nickel oxide, and copper oxide.
[0210] As the conductive layer, a copper layer having a thickness of 0.5 μm and configured in the same manner as in Experimental Example 1 was used.
[0211] The second blackening layer has a thickness of 0.05 μm and contains nickel, copper, oxides of nickel, and oxides of copper.
[0212] The first and second blackening layers had the same composition, and a laminate substrate was prepared with a reflectance of 14% on the surface of the first blackening layer. The first and second blackening layers had the same composition as in Experimental Example 1-5.
[0213] Next, a resist placement process was carried out. Specifically, a photosensitive resist (manufactured by Asahi Kasei Corporation, product name: AQ-1F59) was attached to the surface of the second blackened layer by a lamination method to form a photosensitive resist layer (photosensitive resist layer formation step).
[0214] The photosensitive resist layer was exposed to ultraviolet light through a glass mask with a predetermined pattern. The glass mask used here was one that had a resist width of 13 μm after development and was capable of forming a lattice pattern of 100 μm squares.
[0215] Furthermore, the unexposed areas were developed by immersing the film in a 1% by mass aqueous sodium carbonate solution at 30° C. for 60 seconds to form a resist pattern (resist pattern formation step).
[0216] The laminate substrate having the resist pattern formed on the surface of the second blackening layer was subjected to the following patterning process, in which the laminate substrate was washed with water between each step.
[0217] As a first etching solution, a ferric chloride solution with a concentration of 25 mass % and a temperature of 30° C. was prepared. The prepared laminate substrate was then immersed in the first etching solution for 10 seconds to etch the conductive layer and the second blackened layer (conductive layer etching step).
[0218] Next, as the second etching solution, a hydrochloric acid solution with a concentration of 20 mass% (Experimental Example 4-1) or 30 mass% (Experimental Example 4-2) was prepared for each experimental example, as shown in Table 5. The second etching solution was used at room temperature (25°C). The copper ion concentration and iron ion concentration of the second etching solution were both 0.
[0219] Then, after completing the conductive layer etching step, the laminate substrate was immersed in the second etching solution of each experimental example for 45 seconds (Experimental Example 4-1) or 20 seconds (Experimental Example 4-2) to etch the first blackened layer (first blackened layer etching step).
[0220] Next, the substrate was immersed in an aqueous sodium hydroxide solution with a concentration of 5% by mass and a temperature of 40° C. for 60 seconds to swell, peel and remove the resist pattern, followed by washing with water and drying to obtain a transparent conductive substrate.
[0221] The obtained transparent conductive substrate was observed using an optical microscope to see if there was any residue of the first blackening layer, and the wiring shape (conductive wiring layer shape) and wiring width (conductive wiring layer width) were measured using an electron microscope.
[0222] The wiring width was measured for four arbitrarily selected wirings, and the average value was regarded as the wiring width of the transparent conductive substrate.
[0223] The evaluation results are shown in Table 5. Moreover, Fig. 8 shows an electron microscope photograph of the transparent conductive substrate including the lattice-shaped thin metal wires obtained in Experimental Example 4-1.
[0224] [Table 5] From the results shown in Table 5, it was confirmed that in both Experimental Example 4-1 and Experimental Example 4-2, there was no residue of the first blackening layer, and good etching was performed without peeling or damage to the mesh wiring. In other words, it was confirmed that the blackening layer and the conductive layer could be patterned into the desired shape. In addition, when the obtained transparent conductive substrate was observed by SEM, it was confirmed that in both Experimental Example 4-1 and Experimental Example 4-2, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less. [Experimental Example 5] Transparent conductive substrates were produced as Experimental Examples 5-1 and 5-2. Both Experimental Examples 5-1 and 5-2 are examples of the present invention.
[0225] In the conductive layer etching step, a cupric chloride solution having a concentration of 21% by mass and a temperature of 35°C was prepared as a first etching solution, and the prepared laminate substrate was immersed in the first etching solution for 45 seconds to etch the conductive layer and the second blackened layer.
[0226] In the first blackening layer etching step, a hydrochloric acid aqueous solution having a hydrochloric acid concentration of 20% by mass (Experimental Example 5-1) or 30% by mass (Experimental Example 5-2), as shown in Table 6 for each experimental example, was prepared as the second etching solution, and the immersion time was 20 seconds (Experimental Example 5-1) or 10 seconds (Experimental Example 5-2).
[0227] Except for the above, a transparent conductive substrate was produced and evaluated in the same manner as in Experimental Example 4. The results are shown in Table 6.
[0228] The second etching solution was used at room temperature (25° C.) The copper ion concentration and iron ion concentration of the second etching solution were both zero.
[0229] [Table 6] From the results shown in Table 6, it was confirmed that in both Experimental Example 5-1 and Experimental Example 5-2, there was no residue of the first blackening layer, and good etching was performed without peeling or damage to the mesh wiring. In other words, it was confirmed that the blackening layer and the conductive layer could be patterned into the desired shape.
[0230] When the obtained transparent conductive substrate was observed by SEM, it was confirmed that in both Experimental Example 5-1 and Experimental Example 5-2, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less. [Experimental Example 6] A transparent conductive substrate was produced. Experimental Example 6 is an example of the present invention.
[0231] First, a laminate substrate having a resist pattern formed on the surface of the second blackening layer was prepared in the same manner as in Experimental Example 4. Then, the following patterning process was carried out on the laminate substrate.
[0232] As the second etching solution, a hydrochloric acid solution with a concentration of 20 mass% was prepared. The second etching solution was used at room temperature (25°C). The second etching solution had a copper ion concentration and an iron ion concentration of 0. The prepared laminate substrate was then immersed in the second etching solution for 45 seconds to etch the second blackened layer (second blackened layer etching step). After the second blackened layer etching step, the substrate was washed with water.
[0233] As the first etching solution, a ferric chloride solution with a concentration of 25% by mass and a temperature of 30° C. was prepared. The laminate substrate on which the second blackening layer etching step had been performed was then immersed in the first etching solution for 10 seconds to etch the conductive layer (conductive layer etching step). After the conductive layer etching step, the laminate was washed with water.
[0234] Next, the laminate substrate that had been subjected to the conductive layer etching step was immersed in the second etching solution for 45 seconds to etch the first blackened layer (first blackened layer etching step). After the first blackened layer etching step, the laminate substrate was washed with water.
[0235] Next, the substrate was immersed in an aqueous sodium hydroxide solution with a concentration of 5% by mass and a temperature of 40° C. for 60 seconds to swell, peel and remove the resist pattern, followed by washing with water and drying to obtain a transparent conductive substrate.
[0236] The obtained transparent conductive substrate was evaluated in the same manner as in Experimental Example 4.
[0237] The evaluation results are shown in Table 7.
[0238] [Table 7] From the results shown in Table 7, it was confirmed that in this experimental example as well, good etching was performed without leaving any residue of the first blackening layer and without peeling or damage to the mesh wiring. In other words, it was confirmed that the blackening layer and the conductive layer could be patterned into the desired shape.
[0239] When the obtained transparent conductive substrate was observed by SEM, it was confirmed that in Experimental Example 6 as well, the protrusion width of the first blackened wiring layer from the conductive wiring layer was 0.5 μm or less. [Experimental Example 7] Transparent conductive substrates were manufactured as Experimental Examples 7-1 to 7-6, with Experimental Examples 7-1 to 7-3 being working examples and Experimental Examples 7-4 to 7-6 being comparative examples.
[0240] First, a laminate substrate was prepared in the same manner as in Experimental Example 1, in which a first blackening layer, a conductive layer, and a second blackening layer were laminated in that order on one side of a transparent substrate, which was a 50 μm-thick polyethylene terephthalate resin (PET) film, to be subjected to the patterning process, except that the film formation conditions of the blackening layer were adjusted so that the film thicknesses of the first and second blackening layers and the reflectance at the surface of the first blackening layer were the desired values.
[0241] The first blackening layer has a thickness of 0.02 μm and contains nickel, copper, nickel oxide, and copper oxide.
[0242] The conductive layer was a copper layer having a thickness of 0.5 μm, and included a conductive thin film layer (copper thin film layer) formed by sputtering and a conductive plating layer (copper plating layer) formed by electroplating.
[0243] The second blackening layer has a thickness of 0.02 μm and contains nickel, copper, nickel oxide, and copper oxide.
[0244] The first and second blackened layers were both formed by reactive sputtering in an atmosphere of argon gas with added oxygen.
[0245] The first blackening layer and the second blackening layer have the same composition in the same laminate substrate, and three types of laminate substrates were prepared with different reflectances at the surface of the first blackening layer, 10%, 14%, and 20%. As shown in Table 8, laminate substrates with a reflectance of 10% at the surface of the first blackening layer were used in Experimental Examples 7-1 and 7-4, laminate substrates with a reflectance of 14% at the surface of the first blackening layer were used in Experimental Examples 7-2 and 7-5, and laminate substrates with a reflectance of 20% at the surface of the first blackening layer were used in Experimental Examples 7-3 and 7-6.
[0246] In each experimental example, the first blackened layer and the second blackened layer were formed by adjusting the film formation conditions, specifically, the voltage applied to the nickel-copper alloy target and the atmosphere, based on a test previously conducted so that the reflectance on the surface of the first blackened layer would be the above-mentioned value.
[0247] As described above, the reflectance on the surface of the first blackening layer means the average reflectance of light having a wavelength of 400 nm or more and 700 nm or less on the surface of the first blackening layer.
[0248] The prepared laminate substrate was cut to an arbitrary size, and then a resist placement step was carried out. Specifically, a dry film resist (manufactured by Asahi Kasei Corporation, product name: ATP-053) was attached to the surface of the second blackened layer by a lamination method to form a photosensitive resist layer (photosensitive resist layer formation step). Then, the photosensitive resist layer was exposed to ultraviolet light, and the unexposed parts were developed to form a resist pattern having a plurality of parallel straight line shapes (resist pattern formation step). Note that the resist pattern had a distance between adjacent lines of 0.1 mm, and a line width (resist width) of 16 μm.
[0249] The laminate substrate having the resist pattern formed on the surface of the second blackening layer was subjected to the following patterning steps, in which the laminate substrate was washed with water between each step.
[0250] The patterning steps of Experimental Examples 7-1 to 7-3 were carried out under the following conditions.
[0251] As a first etching solution, a ferric chloride solution with a concentration of 25 mass % and a temperature of 30° C. was prepared. The prepared laminate substrate was then immersed in the first etching solution for 10 seconds to etch the conductive layer and the second blackened layer (conductive layer etching step).
[0252] Next, a hydrochloric acid solution with a concentration of 25 mass% and a temperature of 30°C was prepared as a second etching solution. The prepared laminate substrate was then immersed in the second etching solution for 20 seconds to etch the first blackened layer (first blackened layer etching step). The second etching solution had a copper ion concentration and an iron ion concentration of 0.
[0253] The patterning steps of Experimental Examples 7-4 to 7-6 were carried out under the following conditions.
[0254] As a first etching solution, a ferric chloride solution with a concentration of 25 mass % and a temperature of 30° C. was prepared. Then, the prepared laminate substrate was immersed in the first etching solution for 50 seconds to etch the first blackened layer, the conductive layer, and the second blackened layer.
[0255] In addition, in Experimental Examples 7-4 to 7-6, etching with the second etching liquid was not performed.
[0256] For each experimental example, after carrying out the above-mentioned patterning process, the substrate was immersed in an aqueous sodium hydroxide solution with a concentration of 5% by mass and a temperature of 40°C for 60 seconds to swell, peel and remove the resist pattern, followed by washing with water and drying to obtain a transparent conductive substrate.
[0257] For the obtained transparent conductive substrate, the maximum value of the protruding width L of the first blackened wiring layer from the conductive wiring layer was evaluated using an SEM.
[0258] The evaluation results are shown in Table 8. SEM images of the periphery of the conductive wiring layers of Experimental Example 7-1 and Experimental Example 7-6 are shown in Fig. 9 and Fig. 10, respectively.
[0259] [Table 8] In Experimental Examples 7-1 to 7-3, it was confirmed that there was no residue of the first blackened layer, and good etching was performed without peeling or loss of the conductive wiring layer. In addition, as shown in Table 7, it was confirmed that the protrusion width L of the first blackened wiring layer was 0.5 μm or less in the transparent conductive substrates obtained in Experimental Examples 7-1 to 7-3. For example, as shown in FIG. 9, in the SEM image of the transparent conductive substrate of Experimental Example 7-1, it was confirmed that only the transparent base material 91 and the second blackened wiring layer 92 were observed, and the protrusion of the first blackened wiring layer from the conductive wiring layer covered with the second blackened wiring layer 92 was not observed.
[0260] On the other hand, in Experimental Examples 7-4 and 7-5, it was confirmed that the first blackened layer was not etched and remained on the entire surface. Also, in Experimental Example 7-6, since the average reflectance of the first blackened layer was high, it was confirmed that it was more reactive to the etching solution than Experimental Examples 7-4 and 7-5, and that it was possible to remove a part of it. However, as shown in FIG. 10, it was confirmed that the first blackened wiring layer 103 protruded from the conductive wiring layer covered with the second blackened wiring layer 102 arranged on the transparent base material 101, and it was confirmed that the maximum protrusion width L of the first blackened wiring layer was 0.9 μm.
[0261] The method for producing a transparent conductive substrate and the transparent conductive substrate have been described above with reference to the embodiments and examples, but the present invention is not limited to the above embodiments and examples. Various modifications and changes are possible within the scope of the gist of the present invention described in the claims.
[0262] This application claims priority based on Japanese Patent Application No. 2017-105836, filed on May 29, 2017, and Japanese Patent Application No. 2017-143963, filed on July 25, 2017, and the entire contents of Japanese Patent Application No. 2017-105836 and Japanese Patent Application No. 2017-143963 are incorporated by reference into this international application. [Explanation of symbols]
[0263] 10A, 10B Laminated board 11, 11A, 11B, 91, 101 Transparent base material 121, 122 Laminate 121A, 122A First blackening layer 121B, 122B conductive layer 122C Second blackening layer 71 Fine metal wire 22, 33, 43, 51A, 51B, 711 Conductive wiring layer 23, 34, 44, 52A, 52B, 712, 103 1st black wiring layer 32, 42, 53A, 53B, 92, 102 2nd black wiring layer 70 Transparent conductive substrate L: Protrusion width of the first blackened wiring layer
Claims
1. a patterning step of patterning a laminate substrate including a transparent substrate, a first blackening layer formed on at least one surface of the transparent substrate and composed only of nickel, copper, an oxide of nickel, and an oxide of copper, and a conductive layer containing copper, laminated in this order from the transparent substrate side, The patterning process includes a conductive layer etching step of etching the conductive layer with a first etching solution capable of dissolving copper; a first blackening layer etching step of etching the first blackening layer with a second etching solution containing chloride ions and water, wherein the second etching solution has a chloride ion concentration of 10 mass% or more in terms of hydrochloric acid.
2. the laminate further has a second blackened layer containing nickel and copper on a surface of the conductive layer opposite to a surface facing the first blackened layer, The method for producing a transparent conductive substrate according to claim 1 , wherein in the conductive layer etching step, the conductive layer and the second blackening layer are etched with the first etching solution.
3. the laminate further has a second blackened layer containing nickel and copper on a surface of the conductive layer opposite to a surface facing the first blackened layer, 2. The method for producing a transparent conductive substrate according to claim 1, wherein the patterning step further comprises a second blackening layer etching step of etching the second blackening layer with the second etching solution before the conductive layer etching step.
4. 4. The method for producing a transparent conductive substrate according to claim 1, wherein the second etching solution contains at least one selected from the group consisting of iron chloride and copper chloride.
5. The second etching solution contains hydrochloric acid and water, The concentration of hydrochloric acid is 10% by mass or more and 37% by mass or less, The method for producing a transparent conductive substrate according to any one of claims 1 to 4, wherein the copper ion concentration is 0.4 mass % or less.
6. The second etching solution contains hydrochloric acid and water, The concentration of hydrochloric acid is 10% by mass or more and 37% by mass or less, The method for producing a transparent conductive substrate according to any one of claims 1 to 5, wherein the iron ion concentration is 0.2 mass % or less.
7. Prior to the patterning step, The method further includes a resist disposing step of disposing a resist on an exposed surface of the laminate opposite to the surface facing the transparent substrate, The resist placement step includes: a photosensitive resist layer forming step of forming a photosensitive resist layer on the exposed surface; and a resist pattern forming step of exposing the photosensitive resist layer to ultraviolet light according to a resist pattern to be formed and developing an unexposed portion to form a resist pattern. The method for producing a transparent conductive substrate according to any one of claims 1 to 6.
8. A transparent substrate; and a thin metal wire disposed on at least one surface of the transparent substrate, The thin metal wire is a first blackened wiring layer composed only of nickel, copper, nickel oxide, and copper oxide; a copper-containing conductive wiring layer and a copper-containing conductive wiring layer are laminated in this order from the transparent base material side, A transparent conductive substrate, in which, when viewed from a direction perpendicular to one surface of the transparent base material, the protruding width of the first blackened wiring layer protruding from the conductive wiring layer is 0.5 μm or less (excluding those in which undercuts occur).
9. 9. The transparent conductive substrate according to claim 8, wherein the thin metal wire further comprises a second blackened wiring layer containing nickel and copper on a surface of the conductive wiring layer opposite to a surface facing the first blackened wiring layer.
10. 10. The transparent conductive substrate according to claim 8, wherein the average reflectance of the first blackened wiring layer to light having a wavelength of 400 nm or more and 700 nm or less is 15% or less.
Citation Information
Patent Citations
Transparent conductive film and touch panel
JP2003151358A
Sensor panel for large-size display
JP2011018194A
Electrode substrate for touch panel, touch panel, and image display device
JP2013069261A
Wiring forming method and etchant for use in the same
JP2015007271A
Printed wiring board and method for manufacturing the same
JP2015138820A