Crosslinkable and foamable compositions, foams obtained therefrom, compositions for foaming and uses thereof - Patents.com
Hydrogenated styrene-isoprene diblock copolymers combined with ethylene copolymers and blowing agents address the slip resistance and mechanical property challenges of existing outsole materials, producing foams with superior anti-slip and mechanical performance for footwear applications.
Patent Information
- Application Number
- JP2022086354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-07
- Filing Date
- 2022-05-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-05-26
AI Technical Summary
Existing footwear outsole materials, such as EVA foams, lack sufficient slip resistance and balanced mechanical properties, limiting their utility as effective outsoles.
Development of crosslinkable and foamable compositions using hydrogenated styrene-isoprene diblock copolymers, combined with ethylene copolymers and blowing agents, to create foams with enhanced anti-slip properties through peroxide crosslinking and foaming processes.
The resulting foams exhibit excellent anti-slip properties and a balanced mechanical profile, suitable for use in footwear outsoles, with improved performance characteristics.
Smart Images

Figure 0007573566000001 
Figure 0007573566000002 
Figure 0007573566000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of the filing date of U.S. Provisional Patent Application No. 63 / 197,548, filed June 7, 2021, under 35 U.S.C. § 119(e)(1).
[0002] The present disclosure relates to a crosslinkable and foamable composition and a foam obtained by crosslinking and foaming said crosslinkable and foamable composition. [Background technology]
[0003] Various materials are used to make shoe soles, the most prevalent being rubber. Rubber-soled footwear has unparalleled abrasion resistance and greatly improved shrinkage in all seasons, including when walking on wet sidewalks or snow-covered roads. Thermoplastic materials are also used in footwear outsoles. For example, outsoles made of PVC are flexible and inexpensive, but slippery. Thermoplastic elastomer (TPE) compositions are based on materials that behave like cured rubber at room temperature, but are melt-processable at elevated temperatures. The TPE materials most often used to produce shoe soles are styrenic block copolymers (SBC), such as styrene-butadiene-styrene (SBS) triblock copolymers, and thermoplastic polyurethanes (TPU).
[0004] To achieve light weight, foams such as those based on ethylene vinyl acetate (EVA) are also used as footwear outsoles. EVA is widely used to manufacture foam products that are mainly used as midsole parts in footwear applications. However, for outsole use, EVA foam has some drawbacks, such as low slip resistance, which prevents EVA foam from gaining widespread use as footwear outsoles. Blends of various materials are often used to prepare foams with improved anti-slip properties. For example, Chinese Patent No. 104693564 discloses an extensible composition containing bromobutyl (BIIR), EVA and low density polyethylene (LDPE) to make a foam for shoe soles with high damping and anti-slip performance.
[0005] Among TPE materials, SBC such as SBS and SEBS (hydrogenated SBS) are the only category that can be manufactured into lightweight foams in a conventional footwear foam process that involves first incorporating peroxide initiators and chemical blowing agents at a temperature of about 120°C or less, then molding in a mold to crosslink the foam composition, and then foaming at a temperature of about 140°C to 190°C. Foams mainly containing SBC have been developed into foams for shoe soles, since SBC materials also have good overall abrasion and slip resistance. For example, Chinese Patent No. 106349633 discloses an extensible composition mainly containing SEBS and small amounts of LDPE, olefin block copolymer (OBC) and styrene-butadiene rubber (SBR) to make a foam with good dry and wet anti-slip properties. Also, for example, Chinese Patent No. 102888067 discloses an elastic foam material with good elasticity and anti-slip properties mainly containing SEBS and containing PP (polypropylene), EVA, inorganic filler and small amount of filler oil.
[0006] In view of the trend towards using lightweight foams as ground-contact outsoles, there is a continuing need to develop new foaming resins to produce foams with enhanced slip resistance and overall balanced mechanical properties suitable for use as footwear outsole portions, and in view of the popular status of EVA foam for footwear applications, there is a continuing need to modify EVA foam to enhance slip resistance. Summary of the Invention
[0007] The objective of this disclosure is twofold. The first objective is to develop a styrenic block copolymer resin from which foams based have balanced mechanical properties, most specifically excellent anti-slip properties important for footwear outsoles. The foams are produced by incorporating a free radical initiator and a blowing agent into a crosslinkable and foamable composition at a temperature of about 120° C. or less, followed by injection molding of the crosslinkable and foamable composition in an injection mold for peroxide crosslinking and decomposition of the blowing agent at a temperature of about 150° C. to 200° C.
[0008] The second challenge was to develop a styrene block copolymer resin that could be blended with an ethylene-based copolymer, such as EVA, to make a foam that would achieve foam properties that exhibited the benefits of both materials, in particular excellent anti-slip properties that are important for footwear outsole applications.
[0009] The present disclosure is based on the discovery, without being bound by theory, that hydrogenated styrene-isoprene diblock copolymers are ideal for achieving the above-mentioned objectives of the present disclosure. Foams containing hydrogenated styrene-isoprene diblock copolymers achieve desirable anti-slip properties suitable for use as shoe outsoles.
[0010] Still further, the present disclosure is based on the discovery that the polymer structure of hydrogenated styrene-isoprene diblock copolymers is optimal for foam compounding and injection processing, where peroxide initiators and blowing agents are incorporated at temperatures below about 120° C., followed by peroxide crosslinking of the compounds in a mold at temperatures between about 150° C. and 200° C.
[0011] The following provides further details.
[0012] In common practice, SBC is produced by anionic polymerization, first preparing a diblock copolymer of one hard styrene block and one soft block, such as a butadiene or isoprene block, and then forming a linear ABA or star multiblock block copolymer through coupling or sequential polymerization. Hydrogenated SBC, such as SEBS, further enhances mechanical properties and weather resistance. SBC block copolymers as a category of TPEs are widely used in many applications, including footwear foams. Hydrogenated SBC, such as hydrogenated SEBS, is preferred for footwear foam applications. Partially hydrogenated SEBS is most suitable for footwear foam applications, since the residual unsaturation in the soft block promotes peroxide crosslinking.
[0013] In AB type styrenic diblock copolymers, the hard styrene blocks are not linked to form physical crosslinks like multiblock copolymers. It does not have the characteristics of a thermoplastic elastomer, such as elasticity. In short, styrenic diblock copolymers are not considered thermoplastic elastomers and have limited commercial use. For example, few commercial products of styrenic diblock copolymers are available from global SBC producers. Styrenic diblock copolymers are most used in adhesives, coatings or modifiers, where mechanical strength and elasticity are not of primary importance. Unexpectedly and surprisingly, it has been found that AB type hydrogenated styrene-isoprene diblock copolymers can be well formulated and foamed into foams with excellent anti-slip performance.
[0014] It is instructive to further point out the influence of the structural difference between triblock and diblock copolymers on peroxide curing, which is a key treatment to enhance melt strength for foaming. For triblock SEBS, the chemical crosslinks by peroxide crosslinking are introduced at the melt stage to the existing physical crosslinks of SEBS. On the other hand, there is no existing physical crosslink network in styrenic diblock copolymers. In peroxide crosslinking, newly formed crosslinks by peroxide crosslinking are formed and all the free styrene blocks are tightened into the crosslinks. In short, the peroxide crosslinking of styrenic diblock copolymers acts not only to provide chemical crosslinks via peroxide crosslinking but also to form a physical crosslink network as a result of crosslinking. It is also an unexpected surprise that peroxide crosslinking transforms styrene-isoprene diblock copolymers into suitable foaming resins to achieve excellent anti-skid properties.
[0015] In addition, styrene-isoprene diblock copolymers have been found to have good compatibility with other ethylene copolymers such as EVA, which is important in producing foams made from dissimilar polymers. AB diblock copolymers are known to have better self-assembly ability due to the thermodynamic incompatibility between the two AB block copolymers, and this is why AB diblock copolymers are often used as compatibilizers for two dissimilar polymers.
[0016] According to the subject of the present disclosure, the present disclosure provides a crosslinkable and foamable composition, a foam obtained by crosslinking and foaming the same, and the preparation thereof, as described below.
[0017] The present disclosure provides a crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer, a free radical initiator, and a foaming agent. The hydrogenated styrenic diblock copolymer comprises a first block comprising isoprene units and a second block comprising styrene units. Here, the hydrogenated styrenic diblock copolymer comprises 10-60 wt% of styrene units, and 50 mol% or more of the isoprene units are hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 30000-200000. The present disclosure also provides a foam or a footwear component obtained by crosslinking and foaming the above-mentioned crosslinkable and foamable composition. Thus, the obtained foam or the obtained footwear component comprises a hydrogenated styrenic diblock copolymer and has the characteristics of the above-mentioned hydrogenated styrenic diblock copolymer.
[0018] The present disclosure also provides another crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer, an ethylene copolymer, a free radical initiator, and a foaming agent. The characteristics of the hydrogenated styrenic diblock copolymer are as described above and will not be described again. Furthermore, the weight ratio of the ethylene copolymer to the hydrogenated styrenic diblock copolymer is 50 / 50 to 95 / 5. The present disclosure also provides a foam and a footwear component obtained by crosslinking and foaming the above-mentioned crosslinkable and foamable composition. Thus, the obtained foam and the obtained footwear component comprise a hydrogenated styrenic diblock copolymer and an ethylene copolymer, and have the characteristics of the hydrogenated styrenic diblock copolymer and the weight ratio of the ethylene copolymer to the hydrogenated styrenic diblock copolymer described above.
[0019] The present disclosure further provides a composition for foaming, comprising a hydrogenated styrenic diblock copolymer. The characteristics of the hydrogenated styrenic diblock copolymer are as described above, and will not be described again. Furthermore, the present disclosure also provides the use of the above-mentioned composition for preparing a foam.
[0020] The details of one or more embodiments of the disclosure are set forth in the description below. Other features, objects, and advantages of the disclosure will be apparent from the description and the claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Various embodiments of the present disclosure are provided in the following description. These embodiments are intended to describe the technical contents of the present disclosure, and are not intended to limit the scope of the present disclosure. The configurations described in one embodiment can be applied to other embodiments by appropriate modification, substitution, synthesis, or separation.
[0022] In this specification, when a component / ingredient is described as having a certain element, unless otherwise specified, this means that the component / ingredient may have one or more of that element, and does not mean that the component / ingredient has only one of that element.
[0023] In this specification, unless otherwise specified, Feature A "or" or "and / or" Feature B means the presence of Feature A, the presence of Feature B, or the presence of both Feature A and B. Feature A "and" Feature B means the presence of both Feature A and B. The words "comprise(s)", "comprising", "include(s)", "including", "have", "has" and "having" mean "comprise(s) / comprising / comprising including but not limited to".
[0024] In this disclosure, unless otherwise specified, the terms "nearly", "about" and "approximately" refer to an acceptable error in a specified value, typically as determined by one of ordinary skill in the art, depending on how the value is measured or determined. In some embodiments, the terms "nearly", "about" and "approximately" refer to within 1, 2, 3 or 4 standard deviations. In some embodiments, the terms "nearly", "about" and "approximately" refer to within ±20%, ±15%, ±10%, ±9%, ±8%, ±7%, ±6%, ±5%, ±4%, ±3%, ±2%, ±1%, ±0.5%, ±0.05% or less of a given value or range. The quantities given herein are approximate quantities, i.e., "nearly", "about" and "approximately" may be implied without explicitly stating "nearly", "about" and "approximately". Furthermore, the phrases "in the range of a first value to a second value", "in the range of a first value to a second value", "in the range of a first value to a second value", etc., mean that the range includes the first value, the second value, and other values between the first value and the second value.
[0025] Additionally, features of different embodiments of the present disclosure may be mixed together to form other embodiments.
[0026] In some embodiments, the crosslinkable and foamable composition may include a hydrogenated styrenic diblock copolymer, a free radical initiator, and a foaming agent. The hydrogenated styrenic diblock copolymer may include a first block including isoprene units and a second block including styrene units, where the hydrogenated styrenic diblock copolymer includes 10-60 wt. % styrene units, and 50 mol. % or more of the isoprene units are hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 30,000-200,000.
[0027] In some embodiments, the crosslinkable and foamable composition may include a hydrogenated styrene-based diblock copolymer, an ethylene copolymer, a free radical initiator and a foaming agent. The composition of the hydrogenated styrene-based diblock copolymer is as described above and will not be described again. Furthermore, the weight ratio of the ethylene copolymer to the hydrogenated styrene-based diblock copolymer may be 50 / 50 to 95 / 5.
[0028] In some embodiments, foams are provided that are obtainable by crosslinking and foaming any of the above crosslinkable and foamable compositions.
[0029] In some embodiments, footwear components are provided that are obtained by crosslinking and foaming any of the above crosslinkable and foamable compositions.
[0030] In some embodiments, the composition for foaming may include a hydrogenated styrenic diblock copolymer. The composition of the hydrogenated styrenic diblock copolymer is as described above and will not be described again.
[0031] In some embodiments, the use of the above composition for foaming is applied to prepare a foam.
[0032] The components of the crosslinkable and foamable compositions, the components of the foam or footwear obtained by crosslinking and foaming any of the crosslinkable and foamable compositions, and the preparation thereof are described in detail below. In addition, the components of the compositions for foaming are also described in detail.
[0033] Hydrogenated styrenic isoprene diblock copolymer The hydrogenated styrenic diblock copolymers of the present disclosure are diblock copolymers comprising a first block comprising isoprene units and a second block comprising styrene units.
[0034] In some embodiments, the hydrogenated styrenic diblock copolymer may contain about 10-60 wt% styrene units based on the total weight of the hydrogenated styrenic diblock copolymer. When a crosslinked foam is prepared by a crosslinkable and foamable composition having a styrene unit content of less than 10 wt%, the crosslinked foam has poor mechanical properties (e.g., tearability). When a crosslinked foam is prepared by a crosslinkable and foamable composition having a styrene unit content of more than 60 wt%, the crosslinked foam has poor rebound resilience or compression set.
[0035] In some embodiments, for the purpose of producing a crosslinked foam having balanced mechanical properties, the hydrogenated styrenic diblock copolymer may contain about 10-50 wt% styrene units based on the total weight of the hydrogenated styrenic diblock copolymer, with the remainder of the hydrogenated styrenic diblock copolymer being conjugated diene monomer units. Within this range, the crosslinked foam is expected to have balanced mechanical properties and excellent anti-slip properties. In some embodiments, the hydrogenated styrenic diblock copolymer may contain, for example, about 15-50 wt%, 20-50 wt%, 20-45 wt%, 20-40 wt%, or 22-40 wt% styrene units, with the remainder of the hydrogenated styrenic diblock copolymer being conjugated diene monomer units.
[0036] In some embodiments, about 50 mol% or more of the isoprene units of the styrene-based diblock copolymer are hydrogenated after hydrogenation. In some embodiments, about 50-100 mol% of the isoprene units are hydrogenated after hydrogenation. In some embodiments, for example, about 55-100 mol%, 60-100 mol%, 65-100 mol%, 70-100 mol%, 75-100 mol%, or 75-99 mol% of the isoprene units are hydrogenated after hydrogenation. If the hydrogenation degree is less than 50 mol%, the viscosity becomes too high on the metal surface, making production difficult.
[0037] In some embodiments, the hydrogenated styrenic diblock copolymer may have a weight average molecular weight of about 30,000 to 200,000. If the weight average molecular weight of the hydrogenated styrenic diblock copolymer is less than 30,000, the hydrogenated styrenic diblock copolymer provides poor mechanical properties to the resulting foam. If the weight average molecular weight of the hydrogenated styrenic diblock copolymer is greater than 200,000, the hydrogenated styrenic diblock copolymer becomes difficult to process.
[0038] In some embodiments, the hydrogenated styrenic diblock copolymer may have a weight average molecular weight of, for example, about 40,000 to 200,000, 50,000 to 200,000, 60,000 to 200,000, 70,000 to 200,000, 70,000 to 190,000, 70,000 to 180,000, 70,000 to 170,000, 70,000 to 160,000, 70,000 to 150,000, 70,000 to 140,000, 80,000 to 140,000, 80,000 to 130,000, 90,000 to 130,000, or 100,000 to 130,000.
[0039] In some embodiments, the first block may be a polymer block of isoprene units. In some embodiments, the first block may be a polymer block of isoprene units and butadiene units, the butadiene unit content being 15% by weight or less based on the total weight of the first block.
[0040] In some embodiments, the second block may be a polymer block of styrene units. In some embodiments, the second block may be a polymer block of styrene units and conjugated diene monomer units, and the content of the conjugated diene monomer units may be 15 wt% or less based on the total weight of the second block. In some embodiments, the content of the conjugated diene monomer units may be in the range of about 0.5-15 wt%, 0.5-14 wt%, 0.5-13 wt%, 0.5-12 wt%, 0.5-11 wt%, or 0.5-10 wt%, based on the total weight of the second block. Here, the conjugated diene monomer units may be butadiene units, isoprene units, or a mixture thereof. In some embodiments, the second block may be a polymer block of styrene units and butadiene units, and the content of the butadiene units may be 10 wt% or less based on the total weight of the second block. When the second block is a polymer block containing a small amount (15% by weight or less) of conjugated diene monomer units, the flowability of the hydrogenated styrenic diblock copolymer can be improved.
[0041] In some embodiments, the first block can be a polymeric block of isoprene units and the second block can be a polymeric block of styrene units.
[0042] In some embodiments, the first block may be a polymer block of isoprene and butadiene units, the butadiene content being 15% by weight or less, based on the total weight of the first block, and the second block may be a polymer block of styrene units.
[0043] In some embodiments, the first block may be a polymer block of isoprene units, and the second block may be a polymer block of styrene units and conjugated diene monomer units, the conjugated diene monomer units may be butadiene units, isoprene units or a mixture thereof, and the content of the conjugated diene monomer units may be 15 wt % or less based on the total weight of the second block.
[0044] In some embodiments, the first block may be a polymer block of isoprene and butadiene units, and the content of butadiene units may be 15% by weight or less based on the total weight of the first block. The second block may be a polymer block of styrene and conjugated diene monomer units, and the conjugated diene monomer units may be butadiene units, isoprene units, or a mixture thereof, and the content of conjugated diene monomer units may be 15% by weight or less based on the total weight of the second block.
[0045] In some embodiments, for example, when the first block and / or the second block include isoprene units, the 3,4-vinyl bond content in the isoprene units can be in the range of about 5 to 40 mol % before hydrogenation. In some embodiments, the 3,4-vinyl bond content in the isoprene units can be in the range of about 5 to 35 mol %, 5 to 30 mol %, 5 to 25 mol %, 5 to 20 mol %, or 5 to 15 mol % before hydrogenation.
[0046] In some embodiments, for example, when the first block and / or the second block include butadiene units, the 1,2-vinyl bond content in the conjugated diene monomer units (i.e., butadiene) can be in the range of about 5 to 40 mol % before hydrogenation.
[0047] Here, the term "vinyl linkage" is used to describe the polymer product made when 1,3-butadiene is polymerized via a 1,2-addition mechanism and isoprene is polymerized via a 3,4-addition mechanism. The result is a monosubstituted olefinic vinyl group pendant to the polymer backbone. In the case of anionic polymerization of isoprene, insertion of isoprene via the 3,4-addition mechanism gives gem-dialkyl C=C moieties pendant to the polymer backbone. The effect of 3,4-addition polymerization of isoprene on the final properties of the block copolymer will be similar to that obtained from the 1,2-addition of butadiene.
[0048] The method for producing the styrenic diblock copolymer before hydrogenation of the present disclosure is not particularly limited, and any well-known method can be used. Among the polymerization methods, living anionic polymerization is used, which is carried out in a hydrocarbon solvent and can be initiated by an organic alkali metal compound. For example, the synthesis steps of the above polymer are clearly described in U.S. Pat. No. 7,332,542. The hydrocarbon solvent is not particularly limited, and any well-known solvent can be used. For example, the hydrocarbon solvent can include aliphatic hydrocarbons such as n-hexane, alicyclic hydrocarbons such as cyclohexane, and aromatic hydrocarbons such as xylene. The above hydrocarbon solvents can be used alone or in combination of two or more.
[0049] The initiator is not particularly limited, and initiators such as aliphatic hydrocarbon alkali metal compounds, aromatic hydrocarbon alkali metal compounds, and organic amino alkali metal compounds that are known to have anionic polymerization activity with vinyl aromatic monomers such as styrene and conjugated diene monomers such as isoprene are applicable. The alkali metals used as initiators may include lithium, sodium, and potassium. In some embodiments, the initiator may be an aliphatic hydrocarbon alkali metal such as n-butyl lithium.
[0050] The polymerization process to prepare the styrenic diblock copolymer may be carried out similarly to that used for anionic polymerization. The polymerization may be carried out at a temperature of about 0°C to about 180°C, more preferably about 30°C to about 150°C, and most preferably about 30°C to about 90°C. It may be carried out in an inert atmosphere, preferably nitrogen, and completed under a pressure in the range of about 0.5 to about 10 bar. The polymerization process generally requires less than 12 hours, depending on the temperature, the concentration of the monomer components, the molecular weight of the polymer, etc.
[0051] Hydrogenation of styrenic diblock copolymers can be carried out in known hydrogenation processes.For example, such hydrogenation has been completed using methods such as those reported in US Pat. Nos. 3,595,942 and 3,700,633.These hydrogenation methods employ suitable catalysts.These mentioned catalysts can include alkylaluminum or metals selected from Groups IA, II-A and III-B of the Periodic Table of Elements, in particular metals of Group VIII, such as nickel or cobalt, combined with suitable reducing agents such as hydrides of lithium, magnesium or aluminum.
[0052] The hydrogenation treatment is not particularly limited, but the hydrogenation is usually carried out at a temperature of 0° C. to 180° C., more preferably 30° C. to 150° C. The hydrogen pressure used in this treatment is not particularly limited, but is usually 0.1 to 20 MPa, 0.2 to 15 MPa, or 0.3 to 5 MPa. The reaction time is usually 1 minute to 10 hours, or 10 minutes to 5 hours.
[0053] Hydrogenation can be carried out by batch processing, continuous processing, or a combination thereof. If necessary, catalyst residues can be removed. The hydrogenated polymer can be isolated by pouring into hot water with stirring, and the organic solvent can be removed by steam stripping.
[0054] A typical synthetic method for preparing hydrogenated styrene-isoprene diblock copolymer is briefly described here. First, cyclohexane (as a solvent) and n-butyl lithium (as an initiator) are charged into a reactor equipped with a heater and agitator. Second, isoprene is added to the solvent to carry out anionic polymerization. Third, styrene is added to the reactor and the reaction mixture is further polymerized to form a styrene-isoprene diblock copolymer structure. The block copolymer is then hydrogenated in a pressure vessel using nickel 2-ethylhexanoate / TEAL catalyst and hydrogen gas. After about 50 mol% or more of the isoprene units are hydrogenated, the hydrogenation reaction is terminated. The resulting styrene-isoprene diblock copolymer is washed with hot acidic water to remove the residual catalyst.
[0055] In some embodiments, the microstructure of the isoprene segments of the hydrogenated styrenic diblock copolymer, such as the vinyl bond content and styrene content before hydrogenation, and the hydrogenation degree after hydrogenation can be determined by proton nuclear magnetic resonance ( 1 The weight average molecular weight can be measured using H-NMR (NMR) method. Additionally, the weight average molecular weight can be determined by gel permeation chromatography (GPC).
[0056] Additionally, for the purpose of tailoring foam properties, the hydrogenated styrene-isoprene diblock copolymers of the present disclosure may contain up to 20% by weight of a hydrogenated styrenic multiblock copolymer of similar composition, such as a SEPS triblock. The styrene-isoprene multiblock copolymer may have a styrene content of 10-40% by weight, a weight average molecular weight of about 30,000-80,000, a 3,4-vinyl bond content of 10-30 mol% of the isoprene units before hydrogenation, and a hydrogenation degree of 60-95 mol% of the isoprene units. The exact weight ratio of hydrogenated styrenic multiblock copolymer to hydrogenated styrenic diblock copolymer depends on the foam processing and the foam properties required for the end use.
[0057] Ethylene Copolymer In some embodiments of the present disclosure, the crosslinkable and foamable composition may include the hydrogenated styrenic diblock copolymer and the ethylene copolymer.
[0058] In some embodiments, the weight ratio of the ethylene copolymer to the hydrogenated styrenic diblock copolymer can be 50 / 50 to 95 / 5. In some embodiments, the weight ratio of the ethylene copolymer to the hydrogenated styrenic diblock copolymer can be, for example, 50 / 50 to 90 / 10, 60 / 40 to 90 / 10, 65 / 35 to 90 / 10, or 70 / 30 to 90 / 10.
[0059] In the present disclosure, the ethylene copolymer is not particularly limited, and any known ethylene copolymer may be used. For example, suitable ethylene copolymers include polyethylene (PE), ethylene-vinyl acetate copolymer (EVA) obtained by copolymerization of ethylene and vinyl acetate, and ethylene and C 3-10 It may comprise ethylene-α-olefin based copolymers obtainable by random or block copolymerization of α-olefins or combinations thereof.
[0060] In some embodiments, the ethylene copolymer may be a polyethylene, which may be high density polyethylene, low density polyethylene, or a combination thereof.
[0061] In some embodiments, the ethylene copolymer may be an ethylene-vinyl acetate copolymer, and the vinyl acetate content ranges from about 15 to 40% by weight based on the total weight of the ethylene copolymer, in some embodiments, the vinyl acetate content may range from about 15 to 35%, 15 to 30%, 18 to 30%, or 20 to 30% by weight based on the total weight of the ethylene copolymer.
[0062] In some embodiments, the ethylene copolymer may be an ethylene-α-olefin based copolymer, where the α-olefin may include 1-butene, 1-pentene, 1-hexene, 1-octene, and the like, or combinations thereof.
[0063] Free Radical Initiators In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include a free radical initiator, where the free radical initiator used to crosslink the crosslinkable and foamable composition is not particularly limited, and any well-known free radical initiator may be used.
[0064] In some embodiments, the free radical initiator can be an organic peroxide.
[0065] In some embodiments, the organic peroxide can be selected from the group consisting of dicumyl peroxide, 2,5-dimethyl-2,5-di-(t-butyl peroxy)hexane, bis(1-(tert-butylperoxy)-1-methylethyl)-benzene, and combinations thereof. In some embodiments, the organic peroxide can be bis(1-(tert-butylperoxy)-1-methylethyl)-benzene, although the disclosure is not limited thereto.
[0066] The amount of the free radical initiator is not particularly limited. In some embodiments, the amount of the free radical initiator may be about 0.01 to 10% by weight, 0.01 to 9% by weight, 0.01 to 8% by weight, 0.01 to 7% by weight, 0.01 to 6% by weight, 0.01 to 5% by weight, 0.01 to 4% by weight, 0.05 to 4% by weight, 0.05 to 3% by weight, 0.1 to 3% by weight, 0.1 to 2.5% by weight, 0.1 to 2% by weight, 0.1 to 1.5% by weight, or 0.1 to 1% by weight, based on the total weight of the crosslinkable and foamable composition.
[0067] Foaming Agent In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include a foaming agent. Here, the foaming agent is not particularly limited, and any well-known foaming agent may be used. For example, the foaming agent may be a chemical foaming agent, a physical foaming agent, or a combination thereof.
[0068] In some embodiments, the blowing agent is a chemical blowing agent.
[0069] In some embodiments, the blowing agent is azodicarbonamide (ADCA), bis(1-(tert-butylperoxy)-1-methylethyl)-benzene, 4,4'-oxybis(benzenesulfonylhydrazide), p-toluenesulfonyl semicarbazide, N,N'-dinitrosopentamethylene tetramine, diphenylsulfone-3,3'-disulfonyl hydrazide, The blowing agent may include an organic blowing agent such as DPSDSH, trihydraznotriazine, or a combination thereof, or an inorganic thermally decomposable blowing agent such as sodium bicarbonate, ammonium bicarbonate, sodium carbonate, ammonium carbonate, or a combination thereof, where the organic blowing agent and the inorganic thermally decomposable blowing agent may be used alone or together. In some embodiments, the blowing agent may be azodicarbonamide, although the present disclosure is not limited thereto.
[0070] The amount of the foaming agent used is not particularly limited. In some embodiments, the amount of the foaming agent used may be about 0.5 to 10 wt%, 0.5 to 9 wt%, 0.5 to 8 wt%, 0.5 to 7 wt%, 0.5 to 6 wt%, 0.5 to 5 wt%, or 1 to 5 wt%, based on the total weight of the crosslinkable and foamable composition.
[0071] In some embodiments, the blowing agent can be a physical blowing agent such as nitrogen, carbon dioxide, an alkane, a cycloalkane, a dialkyl ether, a cycloalkylene ether, a fluoroalkane, a hydrofluoroolefin, a hydrochlorofluoroolefin, or a combination thereof.
[0072] Other Additives In some embodiments of the present disclosure, in addition to the above components, the crosslinkable and foamable composition may optionally further include other additives, such as crosslinking coagents, organometallic compounds, fillers, heat stabilizers, weather stabilizers, pigments, etc., if necessary, but the present disclosure is not limited thereto.
[0073] In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include a crosslinking coagent for the purpose of accelerating the rate of crosslinking reaction.For example, the crosslinking coagent may include, but is not limited to, triallyl isocyanurate, triallyl cyanurate, ethylene glycol dimethacrylate, vinyl butyrate, etc.
[0074] In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include an organometallic compound for the purpose of making the crosslinked foam pores finer or more uniform. For example, the organometallic compound may include, but is not limited to, zinc diacrylate or zinc dimethacrylate, which may also act as a crosslinking coagent.
[0075] In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include a filler for cost reduction, hardness or modulus adjustment, or nucleation purposes. For example, the filler may include, but is not limited to, clay, silicon dioxide, talc, titanium dioxide, zinc oxide, calcium carbonate, etc.
[0076] In some embodiments of the present disclosure, for the purpose of enhancing the durability of the foam product, the crosslinkable and foamable composition may further include a heat stabilizer, a weathering stabilizer, or a combination thereof. For example, the heat stabilizer may include a phosphorus-based type heat stabilizer, such as, but not limited to, Irgafos 168. For example, the weathering stabilizer may include a hindered phenol-based type weathering stabilizer, such as, but not limited to, pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate].
[0077] In some embodiments of the present disclosure, the crosslinkable and foamable composition may further include a pigment. For example, the pigment may include, but is not limited to, an azo-type pigment, a phthalocyanine-type pigment, an oxide-type pigment, a chromate-type pigment, a molybdate-type pigment, an inorganic pigment, or carbon black.
[0078] Preparation of Crosslinkable and Foamable Compositions The crosslinkable and foamable composition of the present disclosure can be produced by first melting and blending the above components of hydrogenated styrene diblock copolymer, ethylene copolymer, or combinations thereof, and using a kneader to incorporate free radical initiators and blowing agents, as well as other additives such as fillers. Prior to the addition of the free radical initiators and blowing agents, the operation is carried out below 120°C to avoid premature decomposition of the free radical initiators and blowing agents.
[0079] The melt mixing and blending method is not particularly limited, and known methods can be used. For example, extruders such as single screw extruder, twin screw extruder, multi-screw extruder, Henschel mixer, Banbury mixer, roll mill and kneader can be applied to the present disclosure. In some embodiments, the melt mixing method is carried out by using a kneader.
[0080] The shape of the crosslinkable and foamable composition of the present disclosure after melt mixing is not particularly limited. For example, it can be formed into pellet shape, flake shape, strand shape, chip shape, etc. For example, it can be by mixing the components to form pellets by a granulator, etc. For example, after kneading each component of the composition, a roll mill is used to form a sheet. Thereby, a non-crosslinked and non-foamed expandable sheet is prepared, and the expandable sheet comprises any one of the above crosslinkable and foamable compositions.
[0081] Preparation of crosslinked foams The crosslinkable and foamable compositions provided by the present disclosure can be crosslinked and foamed to obtain the foams of the present disclosure.
[0082] The method of crosslinking and foaming is not particularly limited, and any known method can be used. This is an example in which the crosslinkable and foamable composition of the present disclosure is foamed in a sheet form obtained by forming the crosslinkable and foamable composition into a sheet. The crosslinkable and foamable sheet is cut into a size in the range of 1.0 to 1.2 times the volume of the mold, and then inserted into the mold. In a general foaming operation, the mold is heated at about 150 to 200°C and 30 to 300 kgf / cm. 2 and a holding time of 3-50 minutes. In the mold, the crosslinking reaction is carried out and the foaming agent is decomposed at the same time. After waiting for the holding time and opening the mold, the crosslinkable and foamable composition becomes a crosslinked foam. In the industrial production of foam, an injection molding process can be used in which the crosslinkable and foamable composition is melt-injected into a mold for crosslinking and foaming.
[0083] The crosslinked foam obtained from the crosslinkable and foamable composition has a density of about 0.05 to 0.5 g / cm 3 , for example, 0.1 to 0.5 g / cm 3 , 0.1~0.45g / cm 3 , 0.1~0.4g / cm 3 , 0.1~0.35g / cm 3 , 0.1~0.3g / cm 3 or 0.1 to 0.25 g / cm 3The foam may have a specific gravity (also called density) of about 100 to about 200 mm, although the disclosure is not so limited and the specific gravity of the foam may be adjusted by modifying the components of the crosslinkable and foamable composition.
[0084] The crosslinked foam obtained from the crosslinkable and foamable composition may have a hardness (Asker C) of about 30 to 80. In some embodiments where the foam is obtained from a crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer, the foam may have a hardness (Asker C) of, for example, about 30 to 75, 30 to 70, 30 to 65, 30 to 60, 35 to 60, 35 to 55, or 40 to 55. In some embodiments where the foam is obtained from a crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer and an ethylene copolymer, the foam may have a hardness (Asker C) of about 30 to 75, 30 to 70, 30 to 65, 30 to 60, 35 to 60, 35 to 55, or 40 to 55. However, the present disclosure is not limited thereto, and the hardness (Asker C) of the foam may be adjusted by modifying the components of the crosslinkable and foamable composition.
[0085] The crosslinked foam obtained from the crosslinkable and foamable composition may have a dry static friction coefficient in the range of about 0.5 to 1.8, which can be determined according to ASTM D1894. In some embodiments where the foam is obtained from a crosslinkable and foamable composition including a hydrogenated styrenic diblock copolymer, the foam may have a dry static friction coefficient in the range of about 0.6 to 1.8, 0.6 to 1.7, 0.6 to 1.6, 0.6 to 1.5, 0.6 to 1.4, 0.7 to 1.4, 0.7 to 1.3, 0.8 to 1.3, or 0.8 to 1.0. In some embodiments where the foam is obtained from a crosslinkable and foamable composition including a hydrogenated styrenic diblock copolymer and an ethylene copolymer, the foam may have a dry static friction coefficient in the range of about 0.5 to 1.5, 0.5 to 1.4, 0.5 to 1.3, 0.5 to 1.2, 0.5 to 1.1, 0.5 to 1.0, or 0.5 to 0.9. However, the disclosure is not limited in this respect, and the dry static friction coefficient of the foam may be adjusted by modifying the components of the crosslinkable and foamable composition.
[0086] The crosslinked foam obtained from the crosslinkable and foamable composition may have a wet static coefficient of friction in the range of about 0.5 to 1.5, which can be determined according to ASTM D1894. In some embodiments where the foam is obtained from the crosslinkable and foamable composition including the hydrogenated styrenic diblock copolymer, the foam may have a wet static coefficient of friction in the range of about 0.5 to 1.4, 0.5 to 1.3, 0.5 to 1.2, 0.6 to 1.2, 0.6 to 1.1, 0.7 to 1.1, 0.7 to 1.0, 0.8 to 1.0, or 0.8 to 0.9, for example. In some embodiments where a foam is obtained from a crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer and an ethylene copolymer, the foam may have a wet static friction coefficient in the range of, for example, about 0.5-1.4, 0.5-1.3, 0.5-1.2, 0.5-1.1, 0.5-1.0, 0.5-0.9, 0.5-0.8, or 0.5-0.7, although the disclosure is not so limited and the wet static friction coefficient of the foam may be adjusted by modifying the components of the crosslinkable and foamable composition.
[0087] The foam obtained by the crosslinkable and foamable composition of the present disclosure exhibits an excellent balance of mechanical properties at least in terms of rebound resilience, light weight, permanent compression set and tear resistance. Therefore, the foam obtained by the crosslinkable and foamable composition of the present disclosure can be widely used as a lightweight and flexible material in automobiles, structures, daily necessities and sporting goods.
[0088] In some embodiments, the foams obtained with the crosslinkable and foamable compositions of the present disclosure may be used as components of footwear, such as footwear outsoles.
[0089] In particular, when the specific gravity of the foam decreases, the mechanical properties tend to decrease, but in the present disclosure, it is expected to produce a lightweight crosslinked foam with balanced mechanical properties, particularly suitable for shoe outsoles or sports foam pads.
[0090] Thus, in some embodiments, the foam obtained by crosslinking and foaming the crosslinkable and foamable composition of the present disclosure may be included as a component of footwear, such as a shoe outsole or a sports foam pad, although the present disclosure is not limited thereto. EXAMPLES
[0091] The present embodiment will be described in detail below with reference to examples.Nevertheless, the present embodiment is not limited to these examples.In the examples and comparative examples, the preparation and identification of the components used in the examples and comparative examples and the mechanical property evaluation of the crosslinked foam are carried out by the methods described below.
[0092] The identity of the polymer structure of the hydrogenated styrenic diblock copolymer is determined as follows.
[0093] Molecular weight and molecular weight distribution Both weight average molecular weight (Mw) and number average molecular weight (Mn) were tested and determined by gel permeation chromatography (GPC) instrument. The molecular weight value of the peak in the chromatogram was calculated by the calibration curve of commercial standard polystyrene. The molecular weight distribution (Mw / Mn) was determined based on the weight average molecular weight (Mw) and number average molecular weight (Mn). Further details on the test steps and instrument information are described as follows: The apparatus is a commercial GPC system including PDI and refractive index detectors provided by Waters. In general, tetrahydrofuran (THF) is selected as the solvent. The measurement temperature is maintained at 40°C. The flow rate is 1ml / min and the injection volume is 100μl. The ratio of hydrogenated block copolymer / THF is 3mg / 15cc.
[0094] Styrene content and vinyl bond content The styrene content and vinyl bond content of the hydrogenated styrenic diblock copolymer before hydrogenation were measured using a VARIAN 400 provided by Agilent Technologies. 1 It is measured by H-NMR spectroscopy. Generally, deuterated chloroform is the solvent of choice.
[0095] Hydrogenation Degree The degree of hydrogenation is 1 It may be calculated from the rate of decrease of the unsaturated bond signal in the H-NMR spectrum, and the calculation is described as follows: Hydrogenation degree (mol%) = B / (A+B) x 100% A: number of moles of non-hydrogenated conjugated diene monomer units B: Number of moles of hydrogenated conjugated diene monomer units
[0096] Melt Flow Index MFI (Melt Flow Index) is measured according to ASTM-D1238.
[0097] The novel aspects of the styrenic diblock copolymers were evaluated as follows.
[0098] Compounding capability An open roller mixer (HT-8807) provided by Hung Ta Instrument Co., Ltd. is used to evaluate the compounding capabilities of the diblock and triblock samples used in the examples and comparative examples at temperatures not exceeding 120°C. This simulates the compounding process for footwear which involves incorporating both free radical initiators and chemical blowing agents and injecting the compounds into a press mold for foaming at a temperature that will not cause premature decomposition. The temperature is between 100-120°C to avoid decomposition of the free radical initiators and blowing agents.
[0099] Before starting the compounding process, the rollers are heated to 120°C. Then, the sample is placed between the two rollers of the roller mixer. The material is broken into small pieces and gradually melted to form a band. After the material is transformed from the solid state to the molten state, the molten polymer forms a homogeneous band that adheres to the rotating roller. At that time, the level of compounding difficulty and the observation of the quality of the band can be confirmed and determined. If the sample is not well meltable at that temperature condition, the molten surface will be uneven. At the same time, small and irregularly sized pores can also be observed. On the other hand, if the sample is well meltable at this temperature condition, the molten surface will be smooth and uniform.
[0100] The banding on the roller surface was rated on a scale of 1 to 5, with a rating of 5 indicating the formation of a complete molten film, while a rating of 1 indicated poor banding.
[0101] The mechanical properties of the crosslinked foam were evaluated as follows.
[0102] specific gravity Once crosslinked, the foam was punched out into a circular shape with a diameter of 2.54 cm and a thickness of 1 cm, and the density was measured by an electronic density meter (MS-204S, Mettler Toledo).
[0103] hardness The hardness (Asker C) of the foam once crosslinked was measured using an Asker hardness tester (Type C, manufactured by Polymer Co., Ltd.) according to ASTM D2240, and the value was read within 1 second. The average value (arithmetic mean) of 5 points was taken as the hardness.
[0104] split tear strength The tear strength of the foam, once crosslinked, is determined according to ASTM D3574F.
[0105] Tensile strength The tensile strength at break of the foam, once crosslinked, is determined according to ASTM D412.
[0106] Elongation The elongation at break of the foam, once crosslinked, is determined according to ASTM D412.
[0107] Compression set The crosslinked foam was punched out into a circular shape with a diameter of 2.54 cm and used as a test specimen, which was compressed to 50% thickness. After keeping at 50°C for 6 hours, the pressure was released and the thickness after 1 hour was measured. The magnitude of residual deformation was evaluated.
[0108] Impact Resilience The rebound resilience of the crosslinked foam is determined in a vertical rebound apparatus according to ASTM-D 2632. The rebound resilience is determined as the ratio of the bounce height to the drop height of a metal plunger of a defined mass and shape allowed to be dropped onto the foam specimen.
[0109] Static coefficient of friction The static coefficient of friction of the foam, once crosslinked, is determined according to ASTM D1894.
[0110] The resin compositions of the examples and comparative examples are described below.
[0111] Styrenic block copolymer SEP-1: Hydrogenated styrene-isoprene diblock copolymer A hydrogenated styrene-isoprene diblock copolymer, SEP-1, was prepared and characterized as described below. First, 4800 g of cyclohexane, 7.06 mmol of n-butyllithium, and 2.66 mmol of tetrahydrofuran (THF) were charged into a 10-liter reactor equipped with a heater and stirrer. Second, 534 g of isoprene was added to the reactor to initiate anionic polymerization at a temperature of about 45° C. Third, 313 g of styrene was added to the reactor, and the reaction mixture was further polymerized to prepare a styrene-isoprene diblock copolymer. The content of 3,4-vinyl bonds in the isoprene block was about 9.1 mol%.
[0112] Then, the styrene-isoprene diblock copolymer obtained by the above steps was hydrogenated in a pressure vessel using nickel-2-ethylhexanoate / TEAL catalyst and hydrogen gas. The temperature for hydrogenation was controlled at about 40°C to 100°C. After about 80 mol% of the isoprene block was hydrogenated, the hydrogenation reaction was terminated. Then, the obtained sample was washed with hot acidic water to remove the residual catalyst. Finally, the block copolymer was isolated by coagulation in hot water and then dried. The yield of hydrogenated styrene-isoprene diblock copolymer was about 80%.
[0113] Analysis reveals that it has a styrene content of 37% by weight, a degree of hydrogenation of 80 mol% of the isoprene block, a weight average molecular weight of about 121,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03 and an MFI of 4 measured at 230°C / 5 kgf.
[0114] SEP-2: Hydrogenated styrene-isoprene diblock copolymer SEP-2, prepared and characterized in the same manner as SEP-1, as described below, is a fully hydrogenated styrene-isoprene diblock copolymer having a styrene content of 37% by weight, in which the 3,4-vinyl bond content in the isoprene block was about 9 mol% before hydrogenation, and the hydrogenation degree in the isoprene block was 99 mol%. The diblock copolymer has a weight average molecular weight of about 120,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03, and an MFI of 1.5 measured at 230°C / 5 kgf.
[0115] SEP-3: Hydrogenated styrene-isoprene diblock copolymer SEP-3, prepared and characterized in the same manner as SEP-1, as described below, is a hydrogenated styrene-isoprene diblock copolymer having a styrene content of 25% by weight, in which the 3,4-vinyl bond content in the isoprene block was about 9 mol% before hydrogenation, and the hydrogenation degree in the isoprene block was 84 mol%. The diblock copolymer has a weight average molecular weight of about 118,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03, and an MFI of 2.2 measured at 230°C / 5 kgf.
[0116] SEP-4: Hydrogenated styrene-isoprene diblock copolymer SEP-4, prepared and characterized in the same manner as SEP-1, as described below, is a fully hydrogenated styrene-isoprene diblock copolymer having a styrene content of 25% by weight, in which the 3,4-vinyl bond content in the isoprene block was about 9 mol% before hydrogenation, and the hydrogenation degree in the isoprene block was 98 mol%. The diblock copolymer has a weight average molecular weight of about 119,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03, and an MFI of 0.7 measured at 230°C / 5 kgf.
[0117] SEPS-1: Hydrogenated styrene-isoprene-styrene triblock copolymer SEPS-1 is a hydrogenated styrene-isoprene-styrene triblock copolymer and was prepared as described below.
[0118] First, 4800 g of cyclohexane, 10.2 mmol of n-butyllithium, and 2.66 mmol of tetrahydrofuran (THF) were charged into a 10-liter reactor equipped with a heater and stirrer. Second, 120 g of styrene was added to the solvent to allow anionic polymerization to proceed at a temperature of about 45° C. Third, 560 g of isoprene was added to the reactor until the reaction of isoprene was completed. Fourth, 120 g of styrene was added to the reactor, and when the polymerization of styrene was completed, methanol was added to terminate the polymerization and form a styrene-isoprene-styrene triblock copolymer structure. The styrene-isoprene-styrene triblock copolymer had about 10 mol % 3,4-vinyl bonds in the isoprene block.
[0119] The hydrogenated product was prepared in the same manner as SEP-1. Analysis showed that the resulting hydrogenated styrene-isoprene-styrene triblock had a degree of hydrogenation of 78.8 mol%, a styrene content of 28.8 wt%, a weight average molecular weight of about 95,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03, and an MFI of 0.23 measured at 230°C / 5 kgf.
[0120] SEPS-2: Hydrogenated styrene-isoprene-styrene triblock copolymer SEPS-2, prepared and characterized in the same manner as for preparing SEPS-1, as described below, is a fully hydrogenated styrene-isoprene-styrene triblock copolymer having a styrene content of 28.4 wt.%, in which the 3,4-vinyl bond content in the isoprene block was about 10 mol.%, and the hydrogenation degree was 98.2 mol.%. The triblock copolymer has a weight average molecular weight of about 95,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.03, and an MFI of 0.04 measured at 230°C / 5 kgf.
[0121] EEPS-1: Hydrogenated (butadiene / isoprene)-styrene diblock copolymer A hydrogenated (butadiene / isoprene)-styrene diblock copolymer, EEPS-1, was prepared and characterized as described below. First, 4800 g of cyclohexane, 7.89 mmol of n-butyllithium, and 2.66 mmol of tetrahydrofuran (THF) were charged into a 10-liter reactor equipped with a heater and stirrer. Second, 295 g of isoprene and 197 g of butadiene were added simultaneously to the reactor (controlling the I / B molar ratio at 1.25) to initiate anionic polymerization at a temperature of about 50° C. until the reaction of isoprene and butadiene was completed. Third, 289 g of styrene was added to the reactor, and when the polymerization of styrene was completed, methanol was added to terminate the polymerization and form an (isoprene / butadiene)-styrene diblock copolymer. The 3,4-vinyl bond content in the isoprene block was about 13 mol %, and the 1,2-vinyl bond content in the butadiene block was about 16 mol %.
[0122] The (butadiene / isoprene)-styrene diblock copolymer obtained by the above steps was then hydrogenated in a pressure vessel using nickel 2-ethylhexanoate / TEAL catalyst and hydrogen gas. The temperature for the hydrogenation treatment was controlled at about 50°C to 90°C. When the cumulative amount of absorbed hydrogen reached an amount corresponding to the target hydrogenation degree, the hydrogenation reaction was terminated. The obtained sample was then washed with high-temperature acidic water to remove the residual catalyst. Finally, the block copolymer was isolated by coagulation in hot water and dried. The hydrogenated styrene-based diblock copolymer had a hydrogenation degree of 78.1 mol%, a styrene content of 37.1 wt%, a weight average molecular weight (Mw) of 128,000, a molecular weight distribution (weight average molecular weight / number average molecular weight) of 1.06, and an MFI of 0.63 measured at 230°C / 5 kgf.
[0123] EEPS-2: Hydrogenated (butadiene / isoprene)-styrene diblock copolymer EEPS-2, prepared and characterized in the same manner as EEPS-1, as described below, is a fully hydrogenated (butadiene / isoprene)-styrene diblock copolymer having a styrene content of 37.1 wt%, a degree of hydrogenation of 99.1 mol%, a weight average molecular weight (Mw) of 128,000, a molecular weight distribution (Mw / Mn) of 1.06, and an MFI measured at 230° C. / 5 kgf of less than 0.1.
[0124] Ethylene Copolymer EVA-1: Ethylene-vinyl acetate copolymer EVA-1 is an ethylene-vinyl acetate copolymer with a vinyl acetate content of 25% by weight and a melt flow index of 3 g / 10 min measured at 190° C. / 2.16 kgf, manufactured by USI under the trade name “UE659”.
[0125] organic peroxide Bis(1-(tert-butylperoxy)-1-methylethyl)-benzene (BIPB) (Arkema Group) was used.
[0126] Chemical Foaming Agents Azodicarbonamide (AC) (Kumyang) was used.
[0127] Other Additives Calcium carbonate (Yuncheng Chemical Industrial), ZnO (zinc oxide, Diamonchem International) and stearic acid (Vulchem) were used.
[0128] result Table 1 lists the polymer structure information, melt flow index, and compounding ability ratings for Diblock SEP-1, Diblock EEPS-1, and Triblock SEPS-1 as measured per the compounding ability description in the previous section. [Table 1]
[0129] From the results shown in Table 1, it is clear that the diblock samples SEP-1 and EEPS-1 were well compounded in the roll mill compounding evaluation, forming smooth and transparent bands on the rotating roller. This is quite unexpected, as both SEP-1 and EEPS-1 with high molecular weight and high melt viscosity as indicated by the MFI values measured at 230°C / 5kg can be compounded well. For example, diblock SEP-1 has a Mw of 121000. In comparison, triblock SEPS-1 with a weight average molecular weight of 95000 was very difficult to compound in the roll mill and formed an opaque band on the rotating roller.
[0130] In the following Examples (abbreviated as Ex) and Comparative Examples (abbreviated as Comp Ex), a styrene-based block copolymer was mixed with an organic peroxide and a blowing agent to prepare a crosslinked foam.
[0131] In Example 1, 100 parts by weight of a foaming composition of SEP-1, a partially hydrogenated styrene-isoprene diblock copolymer, 0.4 parts by weight of bis(1-(tert-butylperoxy)-1-methylethyl)-benzene (BIPB) based on the total weight of the resin component (here SEP-1), 3.0 parts by weight of azodicarbonamide (AC) based on the total weight of the resin component, 1 part by weight of zinc oxide based on the total weight of the resin component, 1 part by weight of stearic acid based on the total weight of the resin component, and 10 parts by weight of calcium carbonate based on the total weight of the resin component were mixed and kneaded for 10 minutes in a roll mill with the roll surface temperature set at 120°C. Even though SEP-1 has a weight average molecular weight of about 121,000, it was well blended in the mixture with the other contents of the foaming formulation.
[0132] The compounded composition was then pressed in a press mold at 100 kgf / cm 2 The mixture was then heated at 175°C for 10 minutes at a pressure of 1.0 MPa to obtain a crosslinked foam. The foam properties were then determined according to the above methods. The results are shown in Table 2 below.
[0133] Examples 2-6 were prepared and tested following the same method as Example 1, except that different polymer components and different peroxide contents were used as listed in Table 2. Examples 4-6 were based on blends of EVA and various styrenic-isoprene diblock copolymer resins.
[0134] In Comparative Example 1, an EVA foam was prepared and tested according to the same method as in Example 1.
[0135] Comparative Examples 2-5 were prepared according to the same method as Example 1, except that different polymer components and different peroxide contents were used as listed in Table 3 below. Comparative Examples 2 and 3 were based on mixtures of EVA-1 with partially hydrogenated SEPS-1 triblock and fully hydrogenated SEPS-2 triblock, respectively. Comparative Examples 4 and 5 were based on mixtures of EVA-1 with partially hydrogenated EEPS-1 diblock and fully hydrogenated EEPS-2 diblock, respectively.
[0136] The results of Examples 1 to 6 and Comparative Example 1 are shown in Table 2, and the results of Comparative Examples 2 to 5 are shown in Table 3. [Table 2] [Table 3]
[0137] Comparative Example 1 serves to compare the anti-slip performance with Examples 1-6, which contain a styrenic-isoprene diblock copolymer. As shown in Table 2, all of the foams of Examples 1-6 exhibit superior anti-slip properties to the EVA-1 foam of Comparative Example 1. Furthermore, all of the foams of Comparative Examples 2-5 exhibit lower anti-slip properties than the foams of Examples 3-6. These results indicate that foams prepared with compositions containing a styrenic-isoprene diblock copolymer have improved anti-slip properties.
[0138] In conclusion, the present disclosure provides a crosslinked foam obtained by a crosslinkable and foamable composition comprising the hydrogenated styrene-isoprene diblock copolymer of the present disclosure or a blend of the hydrogenated styrene-isoprene diblock copolymer and an ethylene copolymer of the present disclosure. The crosslinked foam of the present disclosure exhibits excellent anti-slip properties and excellent balance of mechanical properties in terms of at least rebound resilience, light weight, permanent compression set and tear resistance. Furthermore, the crosslinked foam can be suitably used as various molded articles such as shoe midsoles and outsoles, automotive parts, civil engineering and construction applications, home appliance parts, sporting goods, and a wide range of other fields. In particular, the crosslinked foam achieves excellent anti-slip properties, which is an important feature for footwear outsole applications.
[0139] Although the present disclosure has been described in relation to embodiments thereof, it should be understood that many other possible variations and modifications can be made without departing from the spirit and scope of the present disclosure as hereinafter claimed.
Claims
1. A crosslinkable and foamable composition comprising a hydrogenated styrenic diblock copolymer, a free radical initiator, and a foaming agent, the hydrogenated styrenic diblock copolymer being: a first block comprising isoprene units; a second block comprising styrene units; Equipped with the first block is composed of isoprene units and may optionally contain butadiene units, and when the butadiene units are contained, the content of the butadiene units is 15 wt% or less based on the total weight of the first block; The hydrogenated styrenic diblock copolymer comprises 10 to 50 weight % of the styrene units, and 50 mol % or more of the isoprene units and optionally the butadiene units are hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 30,000 to 200,000.
2. 2. The crosslinkable and foamable composition according to claim 1, wherein said first block is a polymer block of isoprene units and said second block is a polymer block of styrene units.
3. 2. The crosslinkable and foamable composition according to claim 1, wherein the first block is a polymer block of isoprene units and butadiene units, and the content of the butadiene units is 15% by weight or less based on the total weight of the first block, and the second block is a polymer block of styrene units.
4. 2. The crosslinkable and foamable composition according to claim 1, wherein the first block is a polymer block of the isoprene unit, the second block is a polymer block of the styrene unit and the conjugated diene monomer unit, the conjugated diene monomer unit is a butadiene unit, an isoprene unit or a mixture thereof, and the content of the conjugated diene monomer unit is 15 wt% or less based on the total weight of the second block.
5. 2. The crosslinkable and foamable composition according to claim 1, wherein the first block is a polymer block of the isoprene unit and the butadiene unit, and the content of the butadiene unit is 15% by weight or less based on the total weight of the first block; the second block is a polymer block of the styrene unit and the conjugated diene monomer unit, and the conjugated diene monomer unit is a butadiene unit, an isoprene unit or a mixture thereof, and the content of the conjugated diene monomer unit is 15% by weight or less based on the total weight of the second block.
6. 2. The crosslinkable and foamable composition according to claim 1, wherein the content of 3,4-vinyl bonds in said isoprene units is in the range of 5-40 mol % before hydrogenation.
7. 2. The crosslinkable and foamable composition of claim 1, wherein 60-100 mol % of said isoprene units are hydrogenated after hydrogenation.
8. 2. The crosslinkable and foamable composition of claim 1, wherein said free radical initiator is an organic peroxide, said organic peroxide being selected from the group consisting of dicumyl peroxide, bis(1-(tert-butylperoxy)-1-methylethyl)-benzene, and combinations thereof.
9. 2. The crosslinkable and foamable composition of claim 1, wherein the foaming agent is a chemical foaming agent, the chemical foaming agent being azodicarbonamide.
10. The crosslinkable and foamable composition of claim 1 further comprising a crosslinking coagent.
11. The crosslinkable and foamable composition according to claim 1, wherein the hydrogenated styrenic diblock copolymer comprises 15-50 wt% of the styrene unit, and 70-100 mol% of the isoprene unit is hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 70000-190000.
12. The crosslinkable and foamable composition according to claim 1, wherein the hydrogenated styrenic diblock copolymer comprises 20-45 wt% of the styrene units, and 70-100 mol% of the isoprene units are hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 70000-150000.
13. 2. The crosslinkable and foamable composition according to claim 1, further comprising an ethylene copolymer, the weight ratio of said ethylene copolymer to said hydrogenated styrenic diblock copolymer being 50 / 50 to 95 / 5.
14. The crosslinkable and foamable composition of claim 13, wherein the ethylene copolymer comprises an ethylene-vinyl acetate copolymer, an ethylene-α-olefin copolymer, or a combination thereof.
15. The crosslinkable and foamable composition according to claim 13, wherein said ethylene copolymer is an ethylene-vinyl acetate copolymer, and the content of vinyl acetate is in the range of 15-40 wt% based on the total weight of said ethylene copolymer.
16. The crosslinkable and foamable composition of claim 13 further comprising a crosslinking coagent.
17. A foam obtained by crosslinking and foaming the crosslinkable and foamable composition according to claim 1.
18. 0.1~0.5g / cm 3 a specific gravity of 0.6 to 1.8, a dry static friction coefficient of 0.5 to 1.5, and a hardness of 30 to 80; The dry static friction coefficient and the wet static friction coefficient were determined according to ASTM D1894; 20. The foam of claim 17, wherein the hardness is measured according to ASTM D2240.
19. 20. The foam of claim 17 which is a component of footwear.
20. 20. The foam of claim 19, which is an outsole of an article of footwear.
21. A foam obtained by crosslinking and foaming the crosslinkable and foamable composition according to claim 13.
22. 0.1~0.5g / cm 3 a foam density of 0.5 to 1.5, a dry static friction coefficient of 0.5 to 1.2, and a hardness of 30 to 80; The dry static friction coefficient and the wet static friction coefficient were determined according to ASTM D1894; 22. The foam of claim 21, wherein the hardness is measured according to ASTM D2240.
23. 22. The foam of claim 21 which is a component of footwear.
24. 24. The foam of claim 23, which is an outsole of an article of footwear.
25. 1. A composition for making a foam comprising a hydrogenated styrenic diblock copolymer, the hydrogenated styrenic diblock copolymer comprising: a first block comprising isoprene units; a second block comprising styrene units; Equipped with the first block is composed of isoprene units and may optionally contain butadiene units, and when the butadiene units are contained, the content of the butadiene units is 15 wt% or less based on the total weight of the first block; The hydrogenated styrenic diblock copolymer comprises 10 to 50 weight percent of the styrene units, and 50 mol% or more of the isoprene units and optionally the butadiene units are hydrogenated, and the hydrogenated styrenic diblock copolymer has a weight average molecular weight of 30,000 to 200,000.
26. 26. The composition of claim 25, further comprising an ethylene copolymer.
27. 26. Use of the composition according to claim 25 for preparing a foam.
Citation Information
Patent Citations
Rubber and plastic sole material with high wear resistance and high elastic resilience and preparation method thereof
CN105419069A
Formula and its production for high-elastic EVA foaming sectional material
CN1982364A
Crosslinked foam
JP1988225638A
Shock absorbing gelatinizing material
JP1997157446A
Vibration-damping resin foam and its production
JP2001026663A