process
By separately forming glass sheets with different thicknesses and lamination at controlled conditions, the process addresses optical distortion issues in laminated glass windshields, achieving improved visual performance and compliance with stringent quality standards.
Patent Information
- Application Number
- JP2022196263
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-01-25
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2038-01-25
AI Technical Summary
Existing methods for producing laminated glass windshields fail to meet stringent optical quality requirements, particularly in automotive applications, leading to increased optical distortion and uneven curvature that amplifies defects with changing mounting angles.
A process involving the separate formation of glass sheets with different thicknesses, using press bending and gravity deflection bending, followed by lamination at specific temperature and pressure ranges, with an intermediate layer to achieve identical curvature and reduce optical distortion.
The process results in laminated glass with reduced optical distortion, meeting stringent optical quality standards and improving visual performance by minimizing curvature differences between inner and outer glass surfaces.
Smart Images

Figure 0007576603000003 
Figure 0007576603000004 
Figure 0007576603000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for preparing a laminated glazing and its use in vehicles. More specifically, the present invention relates to a process for preparing a lightweight laminated glazing, In particular it relates to its use in vehicles as a vehicle windscreen.
[0002] Laminated glass for vehicle windshields is usually made of polyvinyl butyral (PVB) The method includes the steps of: It is known that in the art it is customary to refer to each glass sheet as a "ply." For example, the adhesive layer itself is often also called a "ply" (i.e., the ply of PVB). A glass sheet configured to face the inside of the vehicle in which the laminated glazing is to be installed. The ply is often referred to as the "inner ply", while the ply is the outer ply of the vehicle to which the laminated glazing is attached. The glass sheet that is configured to face the side is often called the "outer ply." The glass sheets are often constructed from soda-lime-silicate glass.
[0003] Each of the glass sheets used in a vehicle laminated glazing is typically It is shaped or bent in one or two mutually perpendicular directions to provide a To bend an initially flat glass sheet to a desired curvature to form a windshield. Many methods are known.
[0004] For example, one known method involves simultaneously bending a pair of initially flat glass sheets to form a One glass sheet is placed on top of the other glass sheet and is coated with a suitable " In this way, the inner ply and The outer glass ply sheet is heated until it can be stretched and then subjected to a gravity bending process. Thus, at the same time, it is bent and therefore formed.
[0005] An alternative method of bending windshield glass sheet is to use different inner and outer plies. The inner and outer plies are individually heated and bent for a suitable period of time, usually in sequence, to form the inner and outer plies. For example, one such method of bending individual flat glass sheets is by bending a The heated flat glass sheets are conveyed between a pair of complementary forming members, and each glass sheet is individually molded. The glass sheets are then cooled, joined and bonded to a suitable material such as PVB. A suitable adhesive interlayer may be used for lamination.
[0006] For example, EP0398759 describes a series of laminated glass sheets made of three layers joined together to form a single laminated glass sheet. The first and second glass sheets are then heated to a temperature of 1000° C. It is described that the sheet is heated in a heating furnace so that the temperature of the sheet becomes substantially uniform.
[0007] WO2004 / 085324A1 describes an asymmetric glass intended for the production of laminated glass. The glass sheets of the glass sheet pair are preheated in a preheating furnace and then pressed in the press bending process. The method of subjecting the bending press to a temperature measuring point at the exit of the bending press is described. This ensures that the glass sheet exhibits uniform bending behavior and achieves uniform recovery during cooling. Guarantee the original strength.
[0008] In US 4,260,408, the glass is first deflected by gravity into the vertical component of bending. It is then pressed against a solid mold to create complex bends. A method of forming a glass sheet by bending a glass sheet with a transverse component of bending is described. In order to minimize the duration of the molding cycle and to transfer the gusset from the contour mold to the undermolding mold, The position of the glass relative to the contour mold may change during the transfer of the glass and during its return to the contour mold. To minimize the possibility of the mold being damaged, certain A speed cycle is provided.
[0009] It is also possible to replace damaged glass in the glass pane. For example, GB2221 424, to increase resistance to penetration through openings fitted with glass panes. The method includes removing glass from an opening containing a glass pane, and or laminated glazing consisting of panes of substantially the same geometric shape (with at least one thermal Cementation with an intermediate layer of plastic material results in a window that is substantially equal in size to the original glass. Thinner quartz glass that has been cut to the correct dimensions and subjected to a chemical tempering treatment. The method is described, characterized in that the glass sheet is replaced by a glass sheet fixed thereto. It has been done.
[0010] However, the optical quality requirements for laminated glazing, especially in automotive applications, are becoming more stringent. This is typical when laminated glass is installed as a windshield in a vehicle. Glass that causes an increase in optical distortion in transmission (when viewed through glass tilted at an angle) Small cosmetic variations in the material are becoming increasingly unacceptable.
[0011] For example, in WO2015 / 092385, at least one ply of interlayer material a first ply of glazing material and a second ply of glazing material joined by A laminated glazing is described that includes a first ply of glazing material having a first composition. a second ply of glazing material having a second composition different from the first composition; The laminated glazing includes a glass sheet having a perimeter extending around the perimeter of the laminated glazing. Edge compression is also present, and edge stress is The magnitude of the surface compressive stress in the surrounding area is greater than the magnitude of the surface compressive stress in the surrounding area. While teaching how to achieve a lightweight windshield, the optical properties required for the lightweight windshield are also No parameters are taken into account.
[0012] In WO2015 / 031594, a first glass layer, a second glass layer, and a first and at least one polymer interlayer between the glass layer and the second glass layer. In some embodiments, the first glass layer comprises first and second glass layers. The glass may be constructed of tempered glass having two surfaces, the second surface being adjacent to the interlayer and having a vitreous layer. The second glass layer is made of tempered glass having a third and fourth surface. The fourth surface faces the intermediate layer and is chemically polished. The surface is adjacent to the intermediate layer and has a substantially transparent coating formed thereon. In an embodiment, the first glass layer is curved and the second glass layer is substantially planar. and is cold formed onto the first glass layer, thereby forming a surface compression layer on the surface of the second glass layer. However, as described in this document and using standard lamination procedures, The optical properties of the laminate structure prepared using this method are not optimal for lightweight laminated glazing. do not have.
[0013] Good transmission optics in a laminated windshield containing two sheets of glass and an interlayer; That is, to achieve a low optical power, two glass sheets, each facing away from the intermediate layer, are used. The surfaces of the sheet (often called surfaces 1 and 4) have as nearly identical curvature as possible. It is known that it should be.
[0014] In addition, Glass Processing Days, 2003, pages 50 2-504, it is known that the installation angle of a vehicle windshield has an effect on the optical properties. It is known, for example, that the amplification of optical power varies with the mounting angle. Therefore, any imperfections present in the windshield are amplified to a much higher extent. As the angle of incidence increases, better optical quality is required. One method of achieving this is to use a laminated windshield that is made of glass with optical properties similar to those of the glass used to make the windshield. Improved optical quality at acceptable commercial cost and yield. Producing quality glass is not always possible.
[0015] To address this problem, and to create a laminated glazing that has reduced optical distortion when installed in a vehicle, Another approach to addressing the problem of manufacturing is described in WO2016 / 030678. In the patent application, the laminated glass sheets are each formed separately between a pair of forming members and then The glass sheet has first and second sheets of glazing material laminated together. The location at which one sheet is bent is strategically offset from the location at which the second sheet of glass material is bent. During the lamination step, the first sheet of glass material may be set horizontally and / or vertically. The sheet may be displaced relative to the second sheet of glazing material by a positional displacement in the direction. The first and / or second sheets of material may have at least a portion of their peripheral edges after lamination. may be cut to match.
[0016] However, in WO2016 / 030678, the inventors The glass sheet starts from a position that improves the optical distortion of the windshield. Each of the pieces is produced by the same process and therefore has substantially the same shape and curvature. It is of the following.
[0017] In the automotive industry, laminated glazing has the potential to reduce the overall weight of the glazing unit. There is an ever-increasing need for
[0018] One way to achieve such a lightweight glazing unit is to use asymmetric glass sheets. This means that the individual glass sheets that make up the windshield are of different thicknesses, colors, and , or emissivity. For example, WO2012 / 0730 30, having a thickness in the range of 1.9 to 2.4 mm to provide mechanical strength. The laminate comprises a first ply of glass having a first ply of glass, a polymer interlayer, and a thickness in the range of 0.8 to 1.4 mm. and a second ply of glass that is much thinner than the first ply of glass, thereby reducing the overall weight of the glass pane. A laminated glazing is described which reduces the amount of
[0019] For example, a gravity bending process can be used to achieve the same bending strength in lightweight glazing units of different thicknesses. Alternatively, it is possible to produce glass sheets for use in a different process. and thereby taking advantage of the advantages offered by each of the processes, Capable of producing asymmetrical sheets each for separate use in lath units For example, to ensure good shape and stress level control, a single glass A press bending operation may be used to prepare the outer glass plies of a lightweight glazing unit. However, currently this process does not provide the same quality level. Forming thin glass plies for use in lightweight glazing units at low temperatures It is therefore not possible to use the gravity bending method for the inner ply described in WO2015 / 098385. It is proposed to prepare lightweight glass units by a chemical strengthening process. Unfortunately, this approach is often not feasible with today's modern laminated windshields. This results in a laminated windshield that does not necessarily meet the stringent optical requirements of glass glazing.
[0020] Therefore, the inner and outer glass plies are prepared using different forming processes or tooling. asymmetrical applications, such as windshields, where the glass plies are produced at different times or There is a need for a process that can produce laminated glazing that is both strong and lightweight.
[0021] That is, a glass plate that is asymmetric but has reduced optical distortion when installed in a vehicle. The process of making laminated glass units, such as vehicle windshields, using rye There is a need for a windshield that has an inner region that is specifically designed for improved transmission optics. This shows that.
[0022] According to a first embodiment of the first aspect of the present invention, a process for preparing a laminated glazing is provided. It is i) a first glass sheet formed into a desired shape having a first thickness by a first procedure; providing a ii) forming a second glass sheet having a desired shape and a second thickness by a second procedure; providing a route; iii) providing an interlayer positioned between the first glass sheet and the second glass sheet. Steps and iv) subjecting the first and second sheets of glass to a temperature and pressure sufficient to bond the interlayer material to the glass sheets. and laminating the second glass sheet and the interlayer together; The process comprises: v) after lamination, the shape of the second glass sheet is substantially the same as the shape of the first glass sheet; During lamination to bond the interlayer material to the two glass sheets, the first glass A mold shaped to substantially the same shape as the first glass sheet is applied to a second glass sheet. A process is provided, further comprising the steps:
[0023] In an alternative embodiment of the first aspect of the present invention, a process for preparing a laminated glazing is provided. Seth, i) a first glass sheet formed into a desired shape having a first thickness by a first procedure; providing a ii) forming a second glass sheet having a desired shape and a second thickness by a second procedure; providing a route; iii) providing an interlayer positioned between the first glass sheet and the second glass sheet. and iv) a first and second glass sheet and an interlayer, the interlayer material being interposed between the two glass sheets; Temperatures between 90°C and 132°C and pressures between 8 and 16 bar are used to bond the material to the board. After lamination, the shape of the second glass sheet is similar to that of the first glass sheet. The process is characterized in that the shape of the sintered body is substantially the same as that of the sintered body.
[0024] According to the invention, the thickness of the first glass sheet is different from the thickness of the second glass sheet. Alternatively, the thickness of the first glass sheet may be the same as the thickness of the second glass sheet. However, the process of the present invention preferably involves the use of glass sheets of different thicknesses. When laminating the first and second glass sheets, the thickness of the first glass sheet is preferably less than the thickness of the second glass sheet. applies at different times.
[0025] In the present invention, the inventors have found that the lamination of the first and second glass sheets is preferably 9 It was found to occur at temperatures ranging from 0°C to 132°C and pressures ranging from 8 to 16 bar. Alternatively, the lamination of the first and second glass sheets is preferably performed at a temperature of 95° C. to 130° C. and a pressure in the range of 8 to 16 bar. and lamination of the second glass sheet occurs at a temperature in the range of 100° C. to 130° C. More preferably, the lamination of the first and second glass sheets is performed at 100° C. to 125° C. or 1 It occurs at temperatures ranging from 00°C to 120°C or 95°C to 110°C. However, most Preferably, the lamination of the first and second glass sheets is performed at a temperature in the range of 100° C. to 110° C. All of the above temperature ranges are preferably combined with a pressure in the range of 8 to 16 bar. Used together.
[0026] The lamination step iv) is carried out using vacuum bags and / or rings in an autoclave. This step may then be carried out at a temperature in the range of 80°C.
[0027] Although a variety of suitable interlayer materials may be used, preferably the interlayer is made of polyvinyl butyral. It will be understood that this includes:
[0028] With respect to the first aspect of the invention, the first glass sheet is preferably pressed into a desired shape. That is, for the process according to the first aspect of the present invention, the first glass sheet is The first step used to form the desired shape involves press bending. For the process according to the first aspect of the present invention, forming the second glass sheet into a desired shape. The second procedure used involves gravity deflection bending.
[0029] The thickness of the second glass sheet is preferably within the range of 0.2 mm to 1.4 mm. More preferably, the thickness of the second glass sheet is 0.5 mm to 1.0 mm or 0.5 to 0. The thickness of the second glass sheet is also in the range of 0.5 to 1.2 mm. It may be within the range.
[0030] The thickness of the first glass sheet is preferably within a range of 1.4 mm to 2.5 mm. More preferably, the thickness of the first glass sheet is within the range of 1.6 mm to 2.3 mm. The thickness of the first glass sheet may also be in the range of 1.6 mm to 2.1 mm.
[0031] According to a first embodiment of the first aspect of the present invention, the process preferably comprises the steps of: v) applying a mold to the second glass sheet during lamination, the mold comprising: The method further includes forming the first glass sheet into substantially the same shape as the first glass sheet.
[0032] The mold may be composed of glass, ceramic, or metal. Alternatively, the mold is made of glass. In the method, the mold preferably includes a third glass sheet having substantially the same shape as the first glass sheet. Includes seat.
[0033] Preferably, the third glass sheet is used in laminating the first and second glass sheets. It is formed into the desired shape by press bending beforehand.
[0034] The thickness of the third glass sheet is preferably within the range of 1.4 mm to 2.5 mm. More preferably, the thickness of the third glass sheet is in the range of 1.6 mm to 2.3 mm. The thickness of the third glass sheet may also be in the range of 1.6 mm to 2.1 mm.
[0035] In addition, the first and third glass sheets are preferably bent in a single press bending batch process. Therefore, the first and third glass sheets are preferably prepared in substantially the same manner. The thickness is the same.
[0036] The process according to the first embodiment of the first aspect of the present invention preferably comprises: vi) forming a second glass sheet into substantially the same shape as the first glass sheet prior to lamination; The method further includes providing a foil layer between the mold and the mold.
[0037] That is, the first embodiment of the first aspect of the present invention preferably comprises vi) a second glass sheet. providing a foil layer between the glass sheet and a third glass sheet, is formed into substantially the same shape as the first glass sheet.
[0038] The foil layer preferably has a thickness of 0.05 mm to 0.2 mm. In addition, the foil layer preferably Suitable non-adhesive films include the foil layer, the second glass sheet, and ensures that the third glass sheet is easily separated after the lamination process. The non-stick foil layer film material includes polyester.
[0039] Thus, and with respect to the first aspect of the invention, after lamination is completed, a third glass sheet and The metal and foil layers are then removed from the laminated first and second glass sheets. Preferably, after lamination, the foil layer and the first glass (preferably in the form of a third glass sheet) are The mold is formed to substantially the same shape as the sheet, and the first and second sheets are laminated in a single step. It is removed from the second glass sheet.
[0040] Thus, according to a first aspect of the present invention there is provided a laminated glazing comprising: the first glass sheet includes a first glass outer surface and a first glass sheet inner surface; The second glass sheet includes a second glass sheet outer surface and a second glass sheet inner surface. , The first glass sheet inner surface and the second glass sheet inner surface are located closest to the interlayer. , For a given point on a laminated glazing, the thickness of the laminate produced by the process of the first aspect of the invention is The curvature of the first glass sheet and the curvature of the second glass sheet at a given point on the laminated glass are The difference between the optical powers in transmission is significantly lower and is therefore acceptably low. Preferably, a laminated glazing is provided, i.e. the laminated glazing is The distortion seen by the driver of the fitted vehicle is low.
[0041] That is, the laminated glazing prepared according to the process of the first aspect of the invention comprises two identical Values recorded for laminated glass prepared by laminating a single glass sheet It is preferred to demonstrate optical power values in transmission of 130% or less.
[0042] In such cases, the optical power in transmission of the laminated glazing shall be in accordance with the ECE R43 standard. by the devices described therein or by the company ISRA Vision AG Or "The requirements to test facilities for inspection of the visual distortion at vehicle panes in transmission" Prepared according to appropriate VDA recommendations, such as A 312 recommendation (March 2015) Measured by the device.
[0043] According to a second aspect of the invention, a vehicle is suitable for use in a vehicle and according to the first aspect of the invention, Prepared according to any of the features described above with respect to the first embodiment or alternative embodiments. The present invention provides a laminated glazing comprising:
[0044] Also according to a second aspect of the present invention, there is provided a vehicle-use vehicle, A laminated glass sheet prepared according to any of the features described above with respect to the first embodiment of the present invention. wherein the glass sheet is formed to substantially the same shape as the first glass sheet during lamination. Laminated glass prepared by a lamination process in which a mold is not applied to a second glass sheet This includes a 37% improvement in optical power compared to the previous model.
[0045] According to a third aspect of the invention, any combination of the features of the first and second aspects of the invention is provided. The present invention provides the use of a laminated glazing prepared according to the method and installed in a vehicle.
[0046] According to the first, second or third aspect of the present invention, the laminated glazing is for use in a vehicle. However, the first, second, or third glass article of the present invention may be any glass article that is The laminated glass according to the embodiment is a vehicle windshield or a vehicle rear window. is preferred.
[0047] Embodiments of the invention will now be described, by way of example only, with reference to the following examples and the accompanying drawings, in which: It is written as: [Brief description of the drawings]
[0048] [Figure 1] FIG. 1 is a simplified cross-sectional view of a laminated glazing prepared according to the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a first embodiment of a method for preparing a laminated windscreen according to a first aspect of the present invention. [Diagram 3] FIG. 2 is a schematic diagram of an alternative embodiment of a method for preparing a laminated windscreen according to the first aspect of the present invention. [Figure 4] 1 is a graphical representation of exemplary curvature measurements recorded on the glass sheets of a laminated windshield. [Diagram 5] 1 is a graphical representation illustrating an exemplary comparison of curvature measurements recorded for inner and outer sheets of windshield glass prepared in accordance with the present invention. [Figure 6] 1 is an image of a typical prior art lightweight laminated windshield prepared with inner and outer glass sheets prepared by conventional methods. [Figure 7] 1 is an image of a laminated lightweight windshield prepared according to the method of the present invention. [Figure 8] 1 is a summary flow diagram of a first and second embodiment of a method for preparing a laminated windshield glass sheet according to the present invention.
[0049] In the present invention, the inventors have found that the thickness of one of the glass sheets is greater than that of the second glass sheet. The thickness of the glass sheet is reduced compared to that of the conventional glass sheet, and the glass sheet is carved using different techniques. A vehicle having two curved glass sheets or plies formed into a curved structure. In preparing laminated glazings, such as windshields, modified Using advanced glass processing techniques, thinner glass sheets can be made into thicker, stronger glass sheets. It has been found that it is possible to successfully cast to the curvature and shape of a part.
[0050] The inventors have also reported that, using the procedure described in accordance with the process of the present invention, It has also been found that matching the curved shapes of the two glass sheets in a glass window can be achieved. With reference to and as shown in Figures 2 and 3, respectively, a method according to the present invention The method is further described below by way of example.
[0051] Laminated glazings prepared by each of the methods described below preferably have mutually different curvature directions. The radius of curvature in one or both directions is preferably In general, the distance can be from 300 mm to 8000 mm.
[0052] As illustrated in FIG. 1, a laminated glazing 10 prepared according to the method of the present invention A first ply (or glass sheet) preferably having a concave surface 14 and an opposing convex surface 16. A second ply (or ply) 12 is provided having a convex surface 24 and an opposing concave surface 22. A glass sheet 20 is also provided. The concave surface 14 of the first ply 12 interfaces with an interlayer 25. The convex surface 24 of the second ply 20 also contacts the intermediate layer 25 .
[0053] Using conventional nomenclature, the convex surface 16 of the first ply 12 is the “front surface” of the laminated glazing 10. The convex surface 14 of the first ply 12 is referred to as "Side 1" (or S1). The convex surface 24 of the second ply 20 is called “Surface 2” (or S2). The concave surface 22 of the second ply 20 is called "Surface 3" (or S3) of the laminated glazing 1. 0, called "Surface 4" (or S4).
[0054] In accordance with the present invention, the laminated glazing 10 may be used in a vehicle windshield (front or rear), Whether it is a vehicle glass pane, such as a vehicle sunroof, a vehicle side window, or a vehicle rear window The laminated glazing 10 may also be an architectural glazing.
[0055] Method 1. In FIG. 2, a laminated glazing, such as a vehicle windscreen, is shown according to a first embodiment of the invention. 1 shows a schematic diagram 180 of one embodiment of a first method for preparing
[0056] In the first step of the method, a first glass sheet 120 is formed, for example a windshield glass. The desired shape of the glass sheet is formed into a single sheet of glass. This is done by forming flat glass such as soda lime silicate glass into a single sheet of glass. Utilizing a flat glass sheet, the glass sheet is shaped to have the required edge profile. This can be achieved by cutting the glass sheet into pieces that can then be stretched. The material is then heated to a suitable state and then cast as a whole, for example by press bending.
[0057] In press bending, the process involves the use of a pair of complementary forming dies, an upper forming die and a Press bending generally involves the use of at least one heated forming mold. It involves the use of a mold. A press bending process is used to bend the part, for example, 300 mm in one or more directions. Glass sheet cut to required windshield shape with radius of curvature ~8000mm Form.
[0058] Next, in the first method for preparing a laminated glass sheet according to the present invention, for example, sodalite A second thinner flat sheet 160 of silicate glass is then applied to the glass to obtain the required edge profile. This second glass sheet is also cut into a shape having a groove, for example by gravity or bending. Use the pre-bending process to create the desired front guard with equal or lesser curved shape. It is also cast into the flat glass of the windshield. The required shape is obtained by a molding process different from the process used to mold the A second glass sheet having a lattice shape is achieved.
[0059] In the gravity bending process, precisely sized flat glass sheets or The ply is placed on a bending ring so that the glass can be stretched and bent freely under gravity. The glass is heated to a bending temperature. The bending is achieved by lowering the temperature. In the method of the present invention which seeks to bend thin plies of glass, The second glass sheet, in the shape ultimately required for use in the laminated glazing, is stacked. The force deflection bending process is not fully achieved at this stage.
[0060] Similar to the first glass sheet, a radius of curvature between 300 mm and 8000 mm in one or more directions However, the second glass sheet has a thickness of about 1.0 mm. The second glass sheet is much thinner than the first glass sheet. For example, the thickness of the first glass sheet may be 1.4 mm to 2.5 mm. It may be within the range of 0.5 mm or within the range of 1.6 mm to 2.3 mm. However, , the thickness of the second glass sheet is within the range of 0.2mm to 1.4mm or 0.5mm to 1. The thickness of the first glass sheet may also be in the range of 1.6 mm to 2.0 mm. It may be in the range of 1 mm.
[0061] The first and second pre-cast glass sheets are then secured together by an adhesive interlayer 140. The adhesive intermediate layer is 0.3mm to 1.8mm thick. or the adhesive interlayer may have a thickness range of 0.5 mm to 1.0 mm. Typically, however, the adhesive interlayer material is preferably 0.76 mm thick. Suitable adhesive intermediate layers that can be used in the method of the present invention include, for example, , Polyvinyl chloride (PVC), Polyvinyl butyral (PVB), Poly(ethylene vinyl acetate) Ethylene Vinyl Acetate (EVA), also known as Ethylene Vinyl Acrylate (PEVA), Ethyl Acrylate methyl (EMA), and polyurethane. However, the preferred intermediate layer used in the method of the present invention is polyvinyl butyral (P VB).
[0062] The first and second pre-molded glass sheets 120, 160 are then "pre-molded" together. The adhesive intermediate layer 140 is bonded together in a "pre-nip" process. The adhesive interlayer 140 is then bonded to the glass sheet 120, 160 to remove any air trapped between the glass sheet 120, 160 and the adhesive interlayer 140. The method involves applying a vacuum to the glass sheet and adhesive interlayer combination. Therefore, the air may be removed. Alternatively, the air trapped by compression may be removed. In this case, air may be evacuated from between the glass sheet and the adhesive interlayer.
[0063] In the final step of the method, the glass sheets 120, 160 and adhesive interlayer are An automatic lamination process is used to laminate the glass sheets and interlayers into the desired laminated glass sheet of the required shape. The lamination of the glass sheets and adhesive interlayer is then bonded together in a lamination process. The first method of the present invention is completed using an autoclave. Typical pressure ranges for the lamination process followed are 10 bar to 16 bar for times of 30 to 120 minutes. It is within the range of the rule.
[0064] A typical temperature range for the lamination process according to the first method of the present invention is a time period of 30 to 120 minutes. In other words, the temperature range of the autoclave used in the lamination process is 100°C to 130°C. The oven temperature range is lower than the temperature range typically used for laminating glass sheets.
[0065] By selecting suitable temperature and pressure parameters, polyvinyl butyral (PVB) etc. This allows the interlayer to form a suitable adhesive bond between the glass sheets. The temperature and pressure parameters are preferably such that flow within the laminate structure is minimal, thus resulting in a thinner laminate. To allow the glass sheet or ply to conform to the shape of a thicker glass sheet or ply. are selected in a certain way.
[0066] The laminated glazing 10 prepared according to the method of the present invention is curved in one or more directions. The radius of curvature in each of the one or more directions may be, for example, 300 mm to 8000 mm. If the laminated glazing is curved in two directions, the directions of curvature may be mutually advantageous. is perpendicular to the
[0067] After the lamination stage of the process is complete, a laminated glazing 180, such as a vehicle windshield, is installed. The cells are then removed from the autoclave, washed and packaged ready for use.
[0068] By using the method described above, the inventors have been able to fabricate the outer layer of the thinner second ply 160. The curvature of surface 190 (S4) (the inner surface when placed on a vehicle) and the curvature of the first thicker ply 12 The degree of curvature of the outer surface 195 of the 0 is varied using standard processes and parameters. This achieves a laminated glazing that is less than the same surface area of the plies in a laminated glazing manufactured by It was found that this is possible.
[0069] The curvature of the surface 190 (S4) of the second thinner ply 160 and the curvature of the surface 190 (S4) of the first thicker ply The effect of increasing the curvature of the exterior surface 195 of the vehicle 120 is evident when viewed through a laminated windshield. and the optical distortion, measured as optical power (as described above), is significantly reduced. This is what we should do.
[0070] In Table 1, for preparing a laminated glazing according to the first method of the invention, for example: A summary of the process parameters used in the autoclave is provided. [Table 1]
[0071] By using the method described above with the parameters specified in Table 1, the inventors The method takes advantage of the fact that the thinner inner glass sheet is more flexible than the thicker outer glass sheet. By using the above-mentioned preferred parameters, excellent laminated glazing can be achieved. The range is used to adhere an interlayer (preferably in the form of PVB) to the glass sheet, and the PV B) under conditions that allow for good lamination performance while maintaining the strength of the autoclave. It is also possible to carry out a beam process, which is an important feature of laminated glazing. This is a particularly important feature for laminated glazings used in vehicles.
[0072] More specifically, by using the method of the present invention, two glass sheets and a The interlayer stack is then heated at a typical autoclave pressure of 10-13 bar and at an autoclave temperature of up to temperatures below typical autoclave temperatures of 135°C to 140°C, and 90°C to 132°C Or, it can be understood that this can be achieved by lowering the temperature to 100°C to 130°C. It can be done.
[0073] However, most preferably, the autoclave process in the method of the present invention requires Through careful selection of parameters, two methods for forming a lightweight windshield have been developed. The lamination of glass sheets and interlayers is such that the transmission recorded for such laminated glazing is Optical refractive power (or visible distortion) prepared using standard autoclave conditions in a manner that is significantly reduced compared to the same values recorded for laminated glazing It has been found that this can be achieved.
[0074] Preferably, the recorded optics of the laminated windshield prepared using the method of the present invention The objective power is for a standard windshield with a glass ply thickness of 2.1 mm. Not more than 50% of the same value recorded.
[0075] The optical refractive power recorded for the lightweight laminated glazing prepared by the method of the present invention is Values are also taken from the optical refraction obtained for lightweight laminated glazing prepared by conventional means. This is a significant improvement compared to the force values typically seen for a standard windshield. The optical refractive power exceeds 80% to 110% of the value recorded by the optical
[0076] Method 2. In FIG. 3, a laminated glazing, such as a vehicle windscreen, is shown according to a first embodiment of the invention. A schematic diagram 200 of a second method of adjusting is shown.
[0077] In method 2, a first glass sheet (which may be flat), such as soda-lime silicate glass, is The sheet 220 is then bent, for example by press bending, into a sheet as described with respect to method 1 above. The glass is then formed into the desired shape.
[0078] Next, a second, thinner, flat glass sheet 260 (such as soda-lime-silicate glass) is The second glass sheet is then cut into a shape with the required edge profile. The rod may be, for example, subjected to gravity or flexural bending processes, also as described above with respect to method 1. Thus, the desired windshield glass can be curved to an equal or lesser degree. It is cast, that is, it is used to form the first glass sheet of the windshield glazing. A second glass sheet of the required shape is produced by a forming process different from the process used. The goal is achieved again.
[0079] As in method 1, a radius of curvature of, for example, 300 mm to 8000 mm in one or more directions is applied. The second glass sheet can be cast from the first glass sheet. The glass is much thinner than the original and the two sheets of glass are formed using different techniques. The thickness of the first glass sheet is within the range of 1.4 mm to 2.5 mm or 1.6 mm to 2. However, the thickness of the second glass sheet may be within the range of 0.2 It may be in the range of mm to 1.4 mm or in the range of 0.5 mm to 1.0 mm.
[0080] The first and second cast glass sheets are then assembled with an adhesive interlayer 240. The adhesive interlayer is also as described for method 1 above. The cage may be a polyvinyl chloride cage, preferably having a thickness of 0.76 mm. Additional suitable adhesive intermediates that may be used in the method of the present invention are: The layers may be made of, for example, polyvinyl chloride (PVC), poly(ethylene vinyl acetate) (PEV A) also known as ethylene vinyl acetate (EVA), ethyl methyl acrylate (EMA ), and polyurethanes.
[0081] However, in contrast to Method 1 described above, Method 2 involves the use of two cast glass sheets. and the adhesive interlayer prior to the "pre-nip" stage in which air is expelled from between the adhesive interlayer and the Between the outer surface (S4) 290 of the second glass sheet that is not in contact and the shaped mold 285 , with a modification such that a thin foil layer 280 is applied.
[0082] The thin foil layer 280 is preferably a non-adhesive film that is attached to the second glass sheet 2. 60 and the mold 285 to prevent scratches. Hostophan Films or Mitsubishi Polyester F Hostaphan® and Diafoil® from ilm GmbH Examples of suitable polyester films include, but are not limited to, polyester films available under the trade names I can't.
[0083] The shaped mold 285 preferably matches the profile of the first ply of glass 220. The mold may be made of, for example, plastic, glass, or may be constructed from a suitable material, such as a ceramic material.
[0084] More preferably, however, the mold is the one used to prepare the outer glass sheet 220. The second glass sheet is prepared by the same batch process as the first glass sheet, thereby forming a substantially identical The mold is a glass sheet formed to the same shape as the mold described herein. It is called mold or dependent glass.
[0085] The first and second pre-cast glass sheets 220, 260 are then molded into the mold 200 as shown in FIG. In the arrangement 300, in combination with the thin foil 280 and the subordinate mold or glass 285, The first glass is then combined with an adhesive intermediate layer 240 in a "pre-nip" process. Surface 295 of sheet 220 and surface 298 of dependent mold or glass 285 are "pre-nibbed" A second, thinner glass sheet 260 is attached to the first glass sheet 250 and forms the two outer faces of the "flat" structure. From the first glass sheet side interlayer material 220 and the outer glass sheet 285, 40 and by a thin foil layer 280 on the dependent glass 285 side.
[0086] Thereafter, the voids trapped between the glass sheets 220, 260 and the adhesive interlayer 240 are The air may be extracted using, for example, a vacuum extraction technique or a nip roller process, as in method 1. Remove it as needed.
[0087] The lamination of the glass sheets and adhesive interlayer is then completed using an autoclave. The pressure range used for autoclave lamination in the second method of the present invention is typically The range is 10 bar to 13 bar for a period of 30 to 60 minutes. The temperature range used for lamination is typically 90°C to 132°C for a period of 30 to 60 minutes. The temperature is further within the range of 100° C. to 110° C. A preferred embodiment of the second method according to the present invention is In an embodiment, the temperature of the lamination process is around 105° C. for a duration of approximately 45 minutes. and the pressure may be approximately 10 bar.
[0088] By selecting suitable temperature and pressure parameters in Method 2, polyvinyl butyral can be produced. (PVB) to form a suitable adhesive bond between the glass sheets. That is, the temperature and pressure parameters are preferably selected to minimize flow within the laminate structure. , and therefore thinner glass sheets or plies can be formed in the shape of thicker glass sheets or plies. and also in a way that allows it to follow the shape of the subordinate glass. A vacuum ring or vacuum bag is used to hold the subordinate glass in place during the "screw-up" process. Preferably, if a suitable ion exchanger is used, this may also be used during the autoclave process.
[0089] While an autoclave is preferably used in the lamination process according to the present invention, Those skilled in the art will appreciate that the autoclave process may be performed in accordance with the preferred methods outlined above, if desired. Use the appropriate parameters to automatically pull a vacuum from a vacuum ring or vacuum bag. It will be appreciated that a furnace equipped with a vacuum port may also be utilized in place of the clave. I guess so.
[0090] The resulting laminated glazing may be curved in one or more directions. The radius of curvature in each of the above directions may be 300 mm to 8000 mm. If curved in two directions, the directions of curvature are preferably perpendicular to each other.
[0091] After the lamination process is complete, laminated glass structures, such as windshields, are removed from the autoclave. The glass 285 and the thin film 28 can then be removed from the mold. 0 is removed from the laminated first and second glass sheets to obtain a laminated glass sheet 400. After cleaning, it is ready for use.
[0092] In addition, the use of a thin foil layer 280 allows the inner glass layer 260 to be removed from the subordinate glass mold 285. The surface 290 of the inner glass layer and the subordinate glass mold 286 can be easily separated. The inner surface 284 of the glass mold is also protected from scratches. After separation from the slave glass mold, it is possible to reuse the slave glass mold in a second iteration of Method 2. The subordinate glass mold may be used again as a subordinate mold, or alternatively, The lath mold may be used as the first glass sheet 220. In this method, 2. Since the dependent glass molds can be reused, it avoids the generation of excessive amounts of waste glass. and in addition, the laminated glass prepared by this method has improved optical properties. The present invention provides advantages such as the ability to
[0093] By using the method 2 described above, the inventors were able to obtain a uniform thickness of the inner surface 29 of the second sheet 260. 0 (S4) and the curvature of the outer surface 295 of the first sheet 220 is substantially or almost We have found that it is possible to achieve a laminated glazing that is identical to that described above.
[0094] That is, by using the method of the present invention, the inventors can produce a second, thinner glass The sheet (or inner glass) takes the shape of a first, thicker glass sheet (or outer glass). We found that it is possible to adapt the method to achieve this.
[0095] The inventors have also identified preferred subordinate glasses or molds 285 for use in the methods of the present invention. follows the same profile as the first glass sheet and e.g. Another shaped first glass sheet may be formed in the same press bending batch process as the first glass sheet. I also discovered something.
[0096] The laminated glazing prepared in the above-described embodiments of the present invention is preferably made of a clear float glass. The present invention includes a soda lime silicate glass sheet having a composition such as glass. The glazing also contains iron oxide as a stain to provide a means of solar control in laminated glazing. It may include.
[0097] A typical soda-lime-silicate glass composition is, for example, 69-74 wt. % SiO2, Al 2 O 3 , 10 to 16% by weight of Na 2 O, 0-5% by weight K 2 O, 0-6 wt% Mg O, 5-14 wt% CaO, 0-2 wt% SO 3 , and 0.005 to 2 wt.% F e 2 O 3 may include.
[0098] The glass sheets also contain other additives, such as fining aids, which are typically present in amounts up to 2%. The soda-lime silicate glass composition may also have a characteristic that is characteristic of the glass composition when viewed in transmitted light. To give the desired color, 3 O 4 It may also contain other colorants such as NiO and Se. good.
[0099] Also, the soda-lime silicate glass of each of the glass sheets used in the method of the present invention The compositions may be the same or different.
[0100] In addition, one or more of the glass sheets used in the method of the present invention may be chemically modified. It may be toughened or strengthened by chemical toughening. Thening, for example, involves treating a glass sheet with a potassium salt solution (such as potassium nitrate). The solution is then heated to a temperature in the range of 300°C to 460°C, preferably 4 A temperature in the range of 00°C to 460°C, most preferably a temperature in the range of 420°C to 460°C ( The glass sheet is immersed in potassium salts (approximately 450°C). The sodium ions in the glass sheets are replaced by potassium ions from the solution during lamination. This gives the weapon additional impact resistance.
[0101] Also, according to the method of the present invention, the outer surface S1 is preferably, for example, the periphery of the windshield. In a 300 mm band extending around the It may have compressive stress.
[0102] That is, for example, the convex surface S1 of the first glass sheet 120, 220 of the laminated glazing The compressive stresses are measured using a residual edge compression of less than 11 MPa and an edge compression of more than 25 MPa. The substrate may have edge regions having stresses.
[0103] FIG. 8 illustrates an exemplary method for preparing a laminated glazing, such as a windshield, in accordance with the present invention. A summary flow diagram of the method is provided.
[0104] First, in step 321, a first sheet of, for example, soda-lime-silicate glass is prepared. The soda-lime silicate glass may be clear or tinted. Bright float glass is glass that is manufactured according to BS EN572-1 and EN 572-2, which are incorporated herein by reference. and BS EN572-2 (2004) means a glass sheet having a composition as defined in .
[0105] At step 323, the first glass sheet is cut and then folded using conventional techniques such as press bending. The glass sheet is then molded into the desired overall shape using a special molding technique. For example, the thickness may be in the range of 1.4 to 2.5 mm. The edges of the blade (also known as the outer blank) are smoothed or "edged" and then Wash the lath sheet.
[0106] After cleaning, the glass sheet can be printed on one or both major surfaces depending on the final product requirements. For example, if the final product is a vehicle windshield, the periphery of the glass sheet may be A layer of ink, which may be optically opaque and / or conductive, is printed around the edge of the Shielding bands may be formed as is customary in the art.
[0107] In step 327, the glass sheet is heated in a suitable furnace to the glass softening temperature. The heat-softened glass is then press-bent between a pair of complementary forming members to form the desired outer sheet. Press bending allows precise control of the shape of the glass sheet. Examples of press bending processes and operations are described in WO2005 / 033026A1 and EP0 For example, the cutting of transparent float glass after bending is described in US Pat. The laminated sheet then goes on to serve as the first sheet of a laminated glazing, such as a windshield.
[0108] Upper and / or lower press bending forming members to control the stress in the first glass sheet The outer sheet may be heated to control residual edge stress and / or edge compression. and / or by selecting the temperature required for the lower press bending forming part, e.g. Edge compression with a net stress of less than 25 MPa and residual edge stress with an edge compression of more than 25 MPa It is possible to produce outer sheets having edge regions.
[0109] Residual surface stresses are also reduced by cooling the bent sheet to room temperature immediately after completion of the press bending operation. It can also be controlled by directing cold air around the perimeter of the bent glass sheet before can.
[0110] Direct cold air at the edges of the glass sheet for a suitable length of time to allow it to cool and de-bend. After creating the required residual stresses in the bent glass sheet, in step 329, the bent glass is The sheet is controllably cooled to room temperature in a suitable annealing furnace.
[0111] Bending a series of glass sheets is done by bending several first glass sheets one after the other. In this manner, glass sheets of a batch may be cut into a desired shape and form part of the cutting process. One of the glass sheets may be used as the first glass sheet in a laminated glazing, and may be used in the same batch. Another of the glass sheets was used as a subordinate glass mold during the autoclave procedure described below. You may do so.
[0112] The first glass sheet may be curved in one or more directions. may have a radius of curvature of 300 mm to 8000 mm.
[0113] The second glass sheet of the laminated glazing is produced as follows.
[0114] In step 331, a second sheet of, for example, soda-lime-silicate glass is provided. The soda lime silicate glass may be clear or tinted, or may be soda lime The silicate glass may be modified. In this embodiment, in step 331, A clear float glass sheet is provided.
[0115] The second sheet of soda lime silicate glass is preferably about 0.7 mm thick, for example. 3, and in step 333, the unbent first glass sheet (or outer glass sheet) may have a thickness of 100 mm or more. The blank is cut to have the same perimeter as the soda lime silicate before being bent. The second cut sheet of glass may also be called the inner blank. The second sheet of salt glass may have a thickness of, for example, 0.2 mm to 1.4 mm. The second sheet of soda-lime-silicate glass is, for example, 0.5 mm to 1 mm thick. It is possible.
[0116] At step 335, the second glass sheet is preferably suitably edged and bent. It is washed before being used.
[0117] In step 337, a second glass sheet is preferably placed on a suitable ring mold to form a first The soda-lime silicate glass is then softened and supported on the glass sheet. The second glass sheet is heated to a temperature sufficient to cause it to sag under the influence of gravity. This procedure is conventionally called gravity or flexural bending. The glass is then bent into a first glass sheet. The second wire bends or flexes to a shape that is closer to the shape of the wire. The curvature of the glass sheet may not be the same as the first glass sheet.
[0118] In step 339, the curve is cooled using controlled cooling to reduce the temperature to room temperature. The second glass sheet is then annealed.
[0119] In step 340, for example, the sodium ions in the second glass sheet are typically converted to potassium ions. Soda lime silicate gas is produced using an ion exchange process in which the gas is chemically exchanged with ammonium ions. The bent second glass sheet of the lath may be chemically strengthened.
[0120] It can be difficult to heat strengthen glass sheets with a thickness of 1 mm or less. , the bent second glass sheet of soda-lime-silicate glass may be heat strengthened. It is also expected.
[0121] In step 341, the first glass sheet and the second glass sheet are bent (after steps 321-329). And (after steps 331-340) a curved second glass sheet is provided.
[0122] At step 342, the pair of bent first and second glass sheets are cleaned, 344, with a thickness of 0.3 mm to 1.5 mm, such as polyvinyl butyral A sheet of interlayer material may be placed between the first and second glass sheets. good.
[0123] In this particular embodiment, the interlayer material is preferably 0.76 mm thick polyvinyl chloride. The adhesive interlayer material may be a sheet of polyvinyl chloride (PVB), but other suitable adhesive interlayer materials may be used. This is also fine.
[0124] Alternatively, in step 345, the bent first glass sheet and the second glass sheet are In addition to disposing a suitable interlayer therebetween, a curved second glass layer may be disposed on the opposite side of the interlayer. In addition, a thin foil layer may be placed on the first glass sheet (or outer blank) which is also bent. A mold in the form of a mold (H) may be placed on the thin foil layer on the opposite side to the bent second glass sheet. .
[0125] Thereafter, in step 346, the subordinate mold ( The PVB sheet is placed between them, with an additional bent first glass sheet, etc. The assembly of the first glass sheet and the second glass sheet is subjected to the method 1 or the method 2. and autoclaving the two glass sheets using the preferred conditions defined above. The first glass sheet is attached to the second glass sheet via the PVB which acts as an adhesive between them. It is joined to the
[0126] Thereafter, in step 347, the foil layer and the subordinate mold are removed, and in step 349 If the subordinate mold is in the form of another first glass sheet, it is cleaned, step 341 The glass can be returned to the mold and reused as a bent first glass sheet for lamination or again as a subordinate mold. may be used.
[0127] At step 348, the laminated glass thus produced is washed before being delivered to the customer. and inspect.
[0128] result In order to provide evidence of the proposed beneficial effects of the method according to the first aspect of the present invention, Deflection measurements of the test were used to test laminated glazings and individual glass sheets.
[0129] It is known that the curvatures of both surfaces of a transparent body, and in particular the difference in curvatures, provide the optical refractive power of the transparent body. It is generally known in the art of chemistry.
[0130] Deflection measurement is a reliable procedure used to measure the curvature of shiny surfaces. In flat glass, when the shapes of the inner and outer (or first and second) glass sheets are different, When analyzing flat glass, suppression of signal from the "back" surface, i.e. the surface not intended for analysis Steps are taken to ensure that the adhesive tape is completely removed. This is accomplished by using black adhesive tape. It can be achieved.
[0131] Deflection measurement test methods use sensor technology based on the principle of measuring phase deflection.
[0132] In deflectometry, a field with a sinusoidal profile is used to calculate the local gradient of a surface. A ring pattern is projected onto a white board. A video camera records this pattern through the surface under test. The local gradient of the surface is directly related to the distortion of the observed fringe pattern. This technique requires only one distinction between the data to calculate the curvature. This offers an advantage over range measurements because it allows the user to select the desired measurement. The amplification of high frequency noise is reduced compared to the case of non-range data.
[0133] Therefore, using measuring systems available from the company 3D-Shape GmbH Calculation of the deflectometry used to measure laminated glazing prepared according to the method of the present invention Such systems are also available, for example, from the company ISRA Vision AG. is also available.
[0134] In FIG. 4, a single glass sheet in a laminated glazing such as a windshield or An exemplary graphical representation depicting measurements of the curvature of both plies is shown in FIG. In the representation, the vertical axis is aligned along the vertical line of the windshield shown in the inset photograph shown. The curvature measured by (m -1 The vertical axis is the distance from the top to the bottom of the windshield sheet. The darker lines in graph (A) represent distinct structures. The lighter lines (B) in the graph relate to measurements on the first or outer glass. The second glass ply is smooth in the center but has a noticeable change in curvature in the upper portion of the glass ply. The background of these structures is important to the present invention. For use in the techniques of the present invention, the glass sheets must be Depending on the molding process involved, it may be sufficient to have different characteristics.
[0135] In accordance with the present invention, two sample laminated windshields were prepared according to Method 2 described above. The windshields were visually analyzed and the surface area of each sample (shown in the inset of Figure 4) was The curvature values were measured along the same line. With the inner surface S4 restrained, the laminated windshield the outer (or external) surface of (i.e. the surface exposed to the outside of the vehicle when fitted), i.e. surface S1 With the outer surface S1 restrained, the inner surface of the laminated windshield, i.e., surface S4 was also measured.
[0136] FIG. 5 provides an example of the measurement of the curvature of two glass plies. and the curvature of the outer surface S1 of the outer glass and the curvature of the inner glass (both measured in 1 / m) The curvature of the inner surface S4 is illustrated as a function of vertical position along a vertical line on the glass.
[0137] The results of the curvature measurements are presented in Figure 5. In Figure 5, the darker curve (C) is the outer ( S1) surface, and the lighter colored curve (D) depicts the curvature of the corresponding inner surface S4. From Figure 5, it can be seen that, excluding measurement uncertainties, both surfaces “fit” together. , i.e., it is clear that the curvature of each surface S1 and S4 follows a general profile. In other words, by analyzing the data shown in Figure 5, both S1 and S4 The surface curvature data is 0.0101m on average -1 The maximum difference is only 0.02. 6m-1 Therefore, this data shows that both surfaces have Verify that the results are nearly identical.
[0138] Thus, while it can be seen from FIG. 5 that both surfaces exhibit nearly identical structures, In contrast, FIG. 4 illustrates the equivalent measurement of a single ply of glass, where the ply of glass There is a clear difference in curvature between them.
[0139] As a result of the matching of the curvatures of the inner S4 and outer S1 surfaces of the windshield, The transmission optics of the prepared laminated windshield is significantly improved. The curvature values of sheet S1 were recorded for the inner sheet S4 produced using the method of the present invention. The lens effect, transmission optical distortion, etc. that appears on the laminated windshield substantially matches the curvature value that is set Blurring or clouding is minimal.
[0140] Transmitted optical distortion or haze in laminated windshields produced by the method of the present invention The improvement in the thermal conductivity of the laminated windshield was also observed in the visual inspection of the laminated windshield, as depicted in Figures 6 and 7. This is clear from the comparison.
[0141] FIG. 7 is an image of a laminated lightweight windshield prepared in accordance with the present invention, where the lamination The outer glass sheet of the laminate (220) is formed using a press bending process, while The inner glass sheet (260) is then folded using an alternative procedure, namely the gravity bending process. and the two sheets are laminated according to the method of the present invention.
[0142] FIG. 6 shows how the press-bent outer glass sheet is bent by direct and complete surface contact with the mold. The glass sheet is completely formed into the desired shape by gravity bending. 1 is a pictorial representation of a lightweight laminated windshield prepared by known methods.
[0143] From FIG. 6, it can be seen that the windshield has a mottled appearance with obvious ash deposits across the windshield. It can be seen that there are non-uniform patches of color shading. This gray shading is Such a rapid change in the grey colour of the windshield is particularly evident in the inner area of Rapidly changing optical power in the windshield and therefore undesirable optical effects The nature and number of
[0144] In contrast, visual inspection of the laminated windshield in Figure 7 shows that the laminated windshield has a more uniform color. It can be seen that the front is colored and does not have any mottled shadow spots. The transmission optics of the glass are improved.
[0145] To evaluate the warping effect of laminated windshields produced by the method of the present invention, stack The transmission of light through the multi-layer windshield also reduces the overall optics of the windshield to millidiopters. The measurements were performed using an equipment system capable of measuring (MDPT).
[0146] The instrument system used is capable of measuring optical refractive power. There are several instruments that can perform this function. These systems use a single light source. It works by projecting light from the camera through the windshield onto a white screen. The camera then takes an image of the windshield (called a "silhouette") and The optical power of the glass is calculated in millidiopters.
[0147] In the following evaluation, the refractive power that causes deflection and distortion in the vertical direction (i.e., the vertical component As previously mentioned, the instrument system was designed to comply with the ECE R43 standard. or by the company ISRA Vision AG or requirements to test facilities for inspec tion of the visual distortion at vehicle VDA 312 Recommendations for "panes in transmission" (2 The device is prepared according to the appropriate VDA recommendations, such as the VDA Recommendations of March 2015. do.
[0148] Thus, the optical power of a laminated windshield prepared in accordance with the present invention is Measured using a typical mounting angle of 61° from the vehicle's forward facing position (ECE R43 or VD A312) Report.
[0149] The optical powers of the various laminated windshields were recorded and images were taken as described above. The evaluation results are provided in Table 4. [Table 2]
[0150] Thus, according to the method of the present invention, improved visual appearance and optical parameters can be obtained. It can be appreciated that it is possible to produce a lightweight windshield having
Claims
1. 1. A process for preparing a laminated glazing comprising: i) providing a first glass sheet formed by a first procedure into a desired shape having a first thickness; ii) providing a second glass sheet formed into a desired shape by a second procedure having a second thickness, the thickness of the first glass sheet being different from the thickness of the second glass sheet; iii) providing an interlayer located between the first glass sheet and the second glass sheet; iv) laminating the first and second glass sheets and the interlayer together at a temperature and pressure sufficient to adhere the interlayer to the glass sheets; The process comprising: v) applying a third glass sheet to the second, thinner glass sheet during lamination to bond the interlayer to the two glass sheets such that after lamination, the shape of the second glass sheet is substantially the same as that of the first glass sheet, the third glass sheet having a thickness within the same range as the first glass sheet, formed to substantially the same shape as the first glass sheet, and made in the same batch by the same first procedure as the first glass sheet, and integrated therewith; vi) providing a foil layer comprising a non-adhesive film between the second glass sheet and the integrated third glass sheet formed to substantially the same shape as the first glass sheet prior to lamination.
2. 2. The process of claim 1, wherein in step iv) the lamination occurs at a temperature in the range of 90° C. to 132° C. and a pressure in the range of 8 to 16 bar.
3. 3. The process according to claim 1 or 2, wherein in step iv) the lamination occurs at a temperature in the range of 100°C to 110°C.
4. The process according to any of claims 1 to 3, wherein in step iv) the lamination occurs in an autoclave.
5. The process of any of claims 1 to 4, wherein the intermediate layer comprises polyvinyl butyral (PVB).
6. The process of any of claims 1 to 5, wherein the first step for forming the first glass sheet into the desired shape comprises press bending.
7. The process of any of claims 1 to 6, wherein the second step of forming the second glass sheet into the desired shape comprises gravity bending.
8. The process of any of claims 1 to 7, wherein the second glass sheet has a thickness in the range of 0.2 mm to 1.4 mm.
9. The process of any of claims 1 to 8, wherein the thickness of the first glass sheet is in the range of 1.4 mm to 2.5 mm.
10. The process of claim 1 , wherein the integrated third glass sheet comprises a press bent glass sheet.
11. The process of claim 10, wherein the third glass sheet has a thickness in the range of 1.4 mm to 2.5 mm.
12. The process of any of claims 1 to 11, wherein the first and third glass sheets are prepared in a single press bending batch process.
13. The process according to any of the preceding claims, wherein the foil layer comprises a thickness in the range of 0.05 mm to 0.2 mm.
14. The process of any of claims 1 to 13, wherein the foil layer comprises a non-stick polyester film.
15. The process of any of claims 1 to 14, further comprising the step of: vii) removing the third glass sheet and the foil layer from the laminated first and second glass sheets.
16. A laminated glass sheet that has undergone the process of any one of claims 1 to 15, comprising a 37% improvement in optical refractive power compared to a laminated glass sheet prepared by a lamination process that does not apply a mold shaped to substantially the same shape as the first glass sheet to the second glass sheet during lamination.
17. Use of a laminated glazing prepared as claimed in any one of claims 1 to 15 in a vehicle.
Citation Information
Patent Citations
Manufacture of safety glass
JP1986106237A
Sound absorbing object and its manufacture
JP1998230568A
Polyester film for laminated glass
JP2010159200A
Method for laminating thin glass laminates
JP2015521575A
Photovoltaic glazing
WO2013107706A1