Reinforced platinum alloy, method for producing the reinforced platinum alloy, and glass production apparatus
A reinforced platinum alloy with controlled Zr content and optimized manufacturing process addresses cracking issues in glass manufacturing equipment by balancing high-temperature strength and flexibility, ensuring stable operation and extended lifespan.
Patent Information
- Application Number
- JP2020197842
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Conventional reinforced platinum alloys used in glass manufacturing equipment are prone to unexpected cracking, particularly at the bottom of melting tanks, due to excessive high-temperature strength and machining resistance, leading to reduced lifespan and operational instability.
A reinforced platinum alloy with controlled additive element content, specifically 0.04% to 0.25% Zr, dispersed oxide particles, and optimized manufacturing process to balance high-temperature creep resistance with flexibility, minimizing lattice defects and thermal stress susceptibility.
The alloy exhibits sufficient high-temperature strength and flexibility, preventing cracking and extending the operational life of glass manufacturing equipment, particularly melting tanks, by ensuring a creep rupture time of 100 hours at 1400°C and an elongation at break of 35% or more at room temperature.
Smart Images

Figure 0007576966000003 
Figure 0007576966000004 
Figure 0007576966000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a strengthened platinum alloy suitable as a constituent material for manufacturing equipment for various glass materials, and in particular to a particle-dispersed strengthened platinum alloy containing Zr as an essential additive element and in which oxide particles of the additive element are finely dispersed. [Background technology]
[0002] Conventionally, oxide particle-dispersed reinforced platinum alloys have been used as a component material for manufacturing equipment for various glass materials such as optical glass and glass fiber. In the manufacture of glass materials, molten glass melted at a high temperature of 1000°C or higher is refined and stirred, and then molded and spun. In towers and tanks (melting tanks, etc.), stirring media (stirrs), spinning bushings, etc. that handle such high-temperature materials, good high-temperature strength and high-temperature creep resistance are required to avoid damage such as deformation and cracking at high temperatures. Reinforced platinum alloys are alloy materials in which oxides of additive elements such as Zr, Y, and Ce are finely dispersed in a matrix made of platinum or platinum alloys (PtRh alloys, etc.). Platinum and its alloys, which are the matrix, are high-melting point metals and also have excellent chemical stability. Reinforced platinum alloys, which have increased strength due to particle dispersion strengthening with oxide particles, have higher high-temperature strength and high-temperature creep resistance than platinum, etc. Therefore, deformation and damage during operation of the glass manufacturing apparatus are suppressed, and the risk of contamination of the molten glass is also low.
[0003] As a method for producing a strengthened platinum alloy, a powder metallurgy method is known in which a platinum alloy powder in which oxide particles are dispersed by oxidation is used as a precursor. In the powder metallurgy method, a platinum alloy consisting of platinum and an additive element is first produced by melt casting, and then this is atomized to produce a platinum alloy powder (atomized powder). Then, the platinum alloy powder is oxidized to turn the additive element into oxide particles, and the platinum alloy powder is compression molded and appropriately forged or rolled to produce a strengthened platinum alloy. The applicant of the present application has conducted many studies on strengthened platinum alloys in terms of both the material composition such as the type and composition range of the additive element and the manufacturing process (Patent Documents 1 to 6). And, based on the knowledge obtained from these studies, they have also succeeded in commercializing an effective strengthened platinum alloy for glass manufacturing equipment (for example, the nanoplat (registered trademark) series is an example of a strengthened platinum alloy product by the applicant of the present application). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 06-336631 [Patent Document 2] Japanese Patent Application Publication No. 08-134511 [Patent Document 3] JP 2000-160268 A [Patent Document 4] JP 2006-057164 A [Patent Document 5] WO2002 / 083961 International Publication Pamphlet Summary of the Invention [Problem to be solved by the invention]
[0005] In the above-mentioned conventional techniques, the aim is to increase the high-temperature strength of the strengthened platinum alloy and improve its high-temperature creep resistance by adjusting the material composition and improving the manufacturing process. The conventional strengthened platinum alloys thus completed are applied to the above-mentioned various glass manufacturing apparatuses.
[0006] The glass manufacturing apparatus described above with respect to the application of conventional reinforced platinum alloys operates stably in most cases without any damage such as deformation or cracking. However, it has been confirmed that cracks may occur at unexpected times in some glass manufacturing apparatuses. It has also been confirmed that this particular trouble tends to occur at the bottom of the melting tank for molten glass. When cracks occur in the melting tank, it is possible to continue using the apparatus by repairing it, but this is only temporary and requires the replacement of the apparatus, which is a concern as it will shorten the apparatus's lifespan.
[0007] The cause of the cracking of the reinforced platinum alloys observed in some glass manufacturing equipment is not necessarily clear. This is because the materials in which the cracks occurred are not clearly different in composition from the materials used in other glass manufacturing equipment in which cracks do not occur. In addition, there is no significant difference in the operating conditions, such as the operating temperature and atmosphere, of the various components of the glass manufacturing equipment. Furthermore, the dimensions such as the shape and thickness of each component are designed according to each application, so it is difficult to consider that the operating conditions are the cause.
[0008] The present invention has been made under the above circumstances, and aims to clarify the causes of damage such as cracks that may occur when an oxide dispersion strengthened platinum alloy is applied to a glass manufacturing apparatus, and to provide a glass manufacturing apparatus that can effectively avoid such damage. Another aim is to provide a glass manufacturing apparatus that uses this strengthened platinum alloy. [Means for solving the problem]
[0009] In order to solve the above problems, the present inventors first studied the causes of breakage observed in some glass manufacturing apparatuses. As a result, they considered that conventional reinforced platinum alloys are prone to cracking due to their excessive strength depending on the glass manufacturing apparatus to which they are applied. According to the present inventors, it has been confirmed that the cracking problem of reinforced platinum alloys occurs intensively at the bottom of the melting tank, especially at the bottom periphery. Melting tanks made of reinforced platinum alloys are often manufactured by drawing a plate material. The bottom periphery of the melting tank has an R-shaped cross section, and the degree of processing is particularly high in this part. The reinforced platinum alloy has a higher strength than melting material without dispersed particles due to the dispersion effect of oxides. However, since it has high strength, it can be said that the processing resistance is large and lattice defects such as distortion and dislocation are easily accumulated due to the increase in the degree of processing. Therefore, it can be said that the bottom periphery of the melting tank tends to be a starting point of cracks.
[0010] Then, cracks are generated and propagated by loads caused by temperature changes during operation of the glass manufacturing plant. The melting tank of the glass manufacturing plant is a device for melting glass raw materials to produce molten glass and sending it to the next process, and raw materials may be added to the molten glass during melting. When raw materials are added, the temperature of the molten glass decreases. In addition, the type of glass produced in the glass manufacturing plant is not always the same and is changed according to demand. Therefore, the type of glass melted in the melting tank changes, and such a change in the type of glass also causes a temperature change. Furthermore, the cycle of operation and stop of the device also causes a temperature change. The temperature change in the glass manufacturing device due to the above various factors causes thermal stress. The generation of such thermal stress is not limited to the melting tank. However, as described above, the bottom outer periphery of the melting tank, which includes the starting point of the crack, is easily affected by thermal stress and is considered to be prone to cracks.
[0011] As described above, the present inventors have considered that the cause of cracks occurring in glass manufacturing equipment (melting tanks) is the excessively high strength of the strengthened platinum alloy, which is the material that constitutes the equipment. In this regard, it can be said that the main focus of the development of strengthened platinum alloys in the past has tended to be on improving high-temperature creep properties. However, based on the above considerations, it is difficult to say that simply increasing high-temperature strength is effective. It is considered that, as a means of suppressing the occurrence of cracks, priority should be given to imparting flexibility, and excessive high-temperature strength and high-temperature creep resistance should be suppressed.
[0012] A method for suppressing the high-temperature strength and high-temperature creep resistance of a strengthened platinum alloy is to reduce the content of additive elements and the amount of dispersed particles. However, even if suppression of high-temperature strength and high-temperature creep resistance is necessary to impart flexibility, it is difficult to say that excessive reduction of them is preferable. In particular, in a platinum alloy with too low high-temperature creep resistance, the deformation mode at high temperatures becomes a simple high-temperature deformation, and there is a risk of deformation and damage of the device due to the load alone. In the example of the molten glass melting tank mentioned above, deformation and the like may occur in parts other than the bottom.
[0013] Therefore, the present inventors have approached the problem by reconsidering the manufacturing process in order to develop a strengthened platinum alloy that has flexibility that is less likely to accumulate distortion due to the above-mentioned processing while ensuring sufficient high-temperature creep resistance by minimizing the content of additive elements. As a result of intensive investigation, it has been found that the above-mentioned problems can be solved in a strengthened platinum alloy that has a specified property at high temperature and room temperature while limiting the upper limit of the content of additive elements, and thus the present invention has been conceived.
[0014] The present invention, which solves the above-mentioned problems, is a strengthened platinum alloy comprising a matrix made of a Pt or PtRh alloy and dispersed particles made of an oxide of an additive element, the strengthened platinum alloy essentially containing 0.04 mass % or more and 0.25 mass % or less of Zr as the additive element, with the balance consisting of constituent metals of the matrix, oxygen and unavoidable impurities, and characterized in that the creep rupture time in a high-temperature creep test at 1400°C and a stress of 10 MPa is 100 hours or more and the rupture elongation in a room-temperature tensile test is 35% or more.
[0015] As described above, the strengthened platinum alloy according to the present invention has relatively high high-temperature strength (high-temperature creep resistance) while limiting the content of Zr as an essential additive element to 0.25 mass%. On the other hand, the strengthened platinum alloy according to the present invention is a platinum material having a large tensile elongation (breaking strain) at room temperature and flexibility. The configuration and characteristics of the strengthened platinum alloy according to the present invention will be described below.
[0016] (I) Composition of the strengthened platinum alloy according to the present invention (I-1) Constituent elements and composition of the strengthened platinum alloy according to the present invention The constituent elements of the strengthened platinum alloy according to the present invention are additional elements, of which Zr is an essential additional element, Pt or Pt and Rh, which are constituent elements of the matrix, oxygen, and inevitable impurities. (1)Additional elements The additive elements exist in the form of oxides in the strengthened platinum alloy and contribute to strengthening the alloy as dispersed particles. Zr is an essential additive element because Zr oxide (ZrO2) has a thermal expansion coefficient relatively close to that of Pt. In addition, Zr oxide is less likely to have adverse effects such as coloring on molten glass. Furthermore, Zr has a lower free energy of oxide formation than Pt, so it is easy to form dispersed particles. As described later, in the present invention, it is required to highly oxidize the additive elements contained in trace amounts in the alloy to form ultrafine oxides. In order to meet the above characteristics and requirements, Zr is an essential additive element.
[0017] Zr is an element for strengthening platinum alloys, but is also a useful additive element from the viewpoint of securing tensile elongation (breaking strain) at room temperature related to flexibility. In the present invention, both high-temperature creep properties and room-temperature tensile elongation are set to a certain level or more, and Zr is an essential additive element for obtaining a platinum alloy with such an excellent balance. In this respect, Y and the like, which have been known as additive elements for strengthening platinum, do not have the same effect as Zr. Even if only Y and the like are added instead of Zr, improvement in high-temperature creep properties is observed, but the effect of improving room-temperature tensile elongation is small. As described later, in the present invention, the addition of Y and the like is permitted only as an auxiliary addition together with Zr.
[0018] The content of Zr, which is an essential additive element, is 0.04 mass% or more and 0.25 mass% or less based on the mass of the entire strengthened platinum alloy. If the content of the additive element is less than 0.04 mass%, the strengthening effect of the additive element and its oxide is poor, and high-temperature strength is low. Considering the problem of the present invention, which is to ensure sufficient high-temperature strength, the Zr content must be 0.04 mass% or more.
[0019] Although the high-temperature strength of the strengthened platinum alloy increases with an increase in the Zr content, the high-temperature strength decreases when a certain amount of Zr is added. In addition, when the content of Zr or other additive elements described later increases, there is a concern that the weldability may deteriorate. The deterioration of the weldability is the generation of slag (slag) due to oxides in the weld metal (bead) during welding, the decrease in stability of the molten metal due to oxides, the generation of oxide aggregation, etc. As described above, since the object of the present invention is to ensure sufficient high-temperature strength, it can be said that it is not necessary to add Zr until the high-temperature strength tends to decrease or the weldability deteriorates. Therefore, in the present invention, the upper limit of the Zr content is set to 0.25 mass%.
[0020] The Zr content in the present invention is set to the above range, but the strengthened platinum alloy of the present invention is further characterized by the Zr content within this range, which will be described in detail later in the description of creep strain rate.
[0021] In the present invention, at least one of Y, Ce, Sc, and Hf may be added as an additional element other than Zr. This is because, based on the findings of the applicant, oxide particles of these elements can also act as a strengthening factor for the strengthened platinum alloy to improve the high-temperature creep properties. The amount of these other additional elements added, in terms of the total content with Zr, is 0.04 mass% or more and 0.25 mass% or less. However, the addition of these other additional elements is not essential. In the present invention, the strengthened platinum alloy may be one to which only Zr is added as an additional element.
[0022] (2) Matrix constituent elements (Pt, Rh) The strengthened platinum alloy according to the present invention is a dispersion strengthened alloy with a Pt or PtRh alloy as a matrix. Therefore, Pt or Pt and Rh are the main constituent elements in the present invention. The PtRh alloy is used as the matrix in addition to Pt in order to improve the strength of the matrix. When the matrix is a PtRh alloy, the content of Rh is preferably 5% by mass or more and 40% by mass or less, more preferably 5% by mass or more and 20% by mass or less.
[0023] (3) Oxygen Oxygen exists in the form of oxide together with the additive elements such as Zr in the strengthened platinum alloy. Therefore, oxygen can be said to be an essential element. The oxygen content of the strengthened platinum alloy varies depending on the content of the additive elements, the conditions of the oxidation treatment in the alloy manufacturing process, the content of inevitable impurities in the platinum alloy before the oxidation treatment, and the like. The oxygen content of the strengthened platinum alloy according to the present invention is preferably 1.0 to 2.0 times the theoretical oxygen content resulting from the oxides of the additive elements such as Zr. The theoretical oxygen content is the oxygen atomic concentration in the alloy when it is assumed that all the additive elements in the strengthened platinum alloy have produced oxides. The theoretical oxygen content is calculated based on the content of each additive element, assuming that the oxide of each additive element is an oxide of stoichiometric composition (ZrO2, Y2O3, CeO2, etc.).
[0024] In the present invention, the content of the additive elements is limited to ensure the necessary and sufficient high-temperature strength, and the strength of the strengthened platinum alloy is prevented from becoming excessively high. However, it is not preferable that the strength becomes too low. For this reason, it is necessary to ensure the appropriate strength by making the limited amount of additive elements into oxides as much as possible. In the present invention, when the oxygen content of the strengthened platinum alloy is less than 1.0 times the theoretical oxygen content, the probability of the presence of unoxidized additive elements increases. On the other hand, from the above definition of the theoretical oxygen content, there is a limit to the oxygen that the strengthened platinum alloy can contain. In addition, the presence of oxygen due to the oxidation of inevitable impurities should also be taken into consideration. For this reason, the upper limit of the ratio to the theoretical oxygen content is set to 2.0 times.
[0025] In addition, due to the influence of inevitable impurities, the difference (deviation) between the oxygen content of a strengthened platinum alloy and the theoretical oxygen content tends to become larger as the content of added elements such as Zr becomes lower. This is because, if the raw materials and manufacturing method are the same, it should be considered that the type and content of inevitable impurities are not affected by the amount of added elements. For example, assume that there is a strengthened platinum alloy with a Zr content of 0.04 mass% (400 ppm) and 400 ppm of inevitable impurities. If it is assumed that all of the Zr and inevitable impurities in this strengthened platinum alloy are oxidized, the oxygen content can be 2.0 times the theoretical oxygen content. When a strengthened platinum alloy with a Zr content of 0.08 mass% (800 ppm) is manufactured using the same raw materials and manufacturing process as this strengthened platinum alloy, the content of inevitable impurities will be the same, and if it is assumed that all of the Zr and inevitable impurities are oxidized as above, the oxygen content can be 1.5 times the theoretical oxygen content. As shown in this example, the total oxygen content of a strengthened platinum alloy is affected by inevitable impurities when the amount of added elements is low. However, the ratio to the theoretical oxygen content shown in the above example is merely an example. In reality, the ratio to the theoretical oxygen content may show various values within the range of 1.0 to 2.0 times depending on the type of inevitable impurities and the presence or absence and type of additive elements other than Zr.
[0026] Regarding the oxygen content of strengthened platinum alloys, the oxygen / nitrogen analysis method is currently known as a relatively accurate analytical method, and can be applied to the present invention. Note that, although the oxygen content of the strengthened platinum alloy according to the present invention has some effect on the strength of the alloy, the oxygen content alone does not explain the characteristics of the present invention. This point will be described in detail later.
[0027] (4) Inevitable impurities Examples of the inevitable impurities in the strengthened platinum alloy according to the present invention include Al, Fe, Co, Ni, Si, and W. In addition, precious metals such as Pd, Au, Ag, Ir, and Ru can also be inevitable impurities. Furthermore, when the matrix is Pt (pure Pt), Rh can also be an inevitable impurity in addition to the above. These inevitable impurities originate from the impurities contained in each raw material metal (Pt, Rh) when manufacturing the master alloy, and may also be mixed in from processing equipment such as compression molding and forging. However, as described later, the strengthened platinum alloy according to the present invention can be manufactured by a relatively simple process that does not require wet grinding or degassing of platinum alloy powder, so that the mixing of impurities during the manufacturing process is reduced. The content of these inevitable impurities that are unintentionally contained is preferably 500 ppm or less in total.
[0028] (I-2) Material structure of the strengthened platinum alloy according to the present invention A strengthened platinum alloy is a material structure in which oxide particles are dispersed in a matrix (parent phase) of platinum or a platinum alloy. The strengthened platinum alloy according to the present invention is similar, and oxide particles of additional elements, with Zr being an essential element, are dispersed in a matrix of Pt or PtRh alloy.
[0029] In the present invention, the average particle size of oxide particles that can be measured by a normal observation method is preferably 1 μm or less. Dispersion strengthening by oxide particles works by dispersing fine particles to a high degree. In addition, the lower limit of the average particle size of oxide particles is preferably 0.01 μm or more if oxide particles that can be measured by a normal observation method are the subject. The normal observation method is an observation method using an electron microscope such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM). The particle size can be measured by a biaxial average or a circle equivalent diameter. Since oxide particles in a strengthened platinum alloy often have a shape close to a sphere, there is no need to limit the method for measuring the particle size.
[0030] However, according to the present inventors' estimation, in the strengthened platinum alloy according to the present invention, oxide particles that are difficult to detect by the above-mentioned normal observation method are believed to exist. In the present invention, an extremely small amount of the additive element content is set, and it is believed that the additive element in the mother alloy before oxidation is solid-dissolved in a fine state at the atomic level. Although such additive elements can also generate oxide particles by appropriate oxidation treatment, it is difficult to clearly observe them, and it is difficult to measure their particle size. It is unclear to what extent such ultrafine oxide particles exist compared to oxide particles that can be observed by normal methods. However, the present inventors consider that these ultrafine oxide particles act to improve the material structure of the strengthened platinum alloy and to obtain the flexibility of the material in the room temperature range. The reason why the strengthened platinum alloy has excellent high-temperature strength is not only the dispersion strengthening by the oxide particles, but also the material structure of the matrix. The matrix of the strengthened platinum alloy exhibits a material structure in which leaf-shaped crystal grains with a large aspect ratio are alternately stacked. In the present invention, it is estimated that the above-mentioned ultrafine oxide particles efficiently improve the matrix to such a suitable material structure. It is believed that the effect of such ultrafine oxide particles is exerted simultaneously with the effect (dispersion strengthening) of normal oxide particles, or is exerted separately. Furthermore, since the ultrafine oxide particles are difficult to observe, it is not possible to identify their composition.
[0031] (II) Physical properties of the strengthened platinum alloy according to the present invention As described above, the strengthened platinum alloy according to the present invention is specified by specifying both the creep properties (creep rupture time) in a high-temperature creep test and the tensile properties (rupture elongation) in a room-temperature tensile test.
[0032] (II-1) High temperature creep properties The strengthened platinum alloy according to the present invention is required to have a creep rupture time of 100 hours or more in a high-temperature creep test at 1400°C and a stress of 10 MPa. The strengthened platinum alloy according to the present invention was invented based on the discovery that excessively high high-temperature strength was a cause of problems in conventional strengthened platinum alloys. However, it is not preferable to reduce the high-temperature strength excessively. In the present invention, the creep rupture time in the creep test described above is specified as the necessary and optimal high-temperature strength. The creep test conditions of a temperature of 1400°C and a stress of 10 MPa are set in order to apply a load larger than the operating temperature and applied stress of a melting bath, etc., while assuming these.
[0033] The high-temperature creep properties of the strengthened platinum alloy according to the present invention do not clearly exceed those of conventional strengthened platinum alloys, but are almost comparable to them, with the difference being slight. Since one of the objectives of the present invention is to ensure sufficient high-temperature strength, it is not necessary for the alloy to exhibit clearly superior high-temperature creep properties compared to the conventional technology.
[0034] Incidentally, a general high-temperature creep test can be applied to the measurement and evaluation of the above creep properties. For example, the test method specified in the Japanese Industrial Standard JIS Z 2271 "Method of creep and creep rupture test for metallic materials" can be applied to the high-temperature creep test. From the creep curve (stress-rupture time) obtained by the high-temperature creep test, the rupture time at a specified stress can be measured. The rupture time at the above-mentioned stress of 10 MPa can also be obtained based on the created creep curve. Incidentally, when specifying the rupture time at a stress of 10 MPa, the actual measured value at that stress may be applied, but the rupture time at that stress may also be obtained by extrapolating or interpolating based on the above-mentioned creep curve.
[0035] (II-2) Room temperature tensile properties In addition to the high temperature creep properties, the strengthened platinum alloy according to the present invention is required to have a breaking elongation of 35% or more in a room temperature tensile test. This breaking elongation property indicates the flexibility and softness of the material at room temperature. The strengthened platinum alloy according to the present invention can suppress the accumulation of strain and lattice defects introduced by processing by acquiring flexibility at room temperature. Glass manufacturing equipment such as melting tanks are usually manufactured by processing at room temperature. As described above, melting tanks are often manufactured by drawing, and the degree of processing of the bottom outer periphery is high. According to the present invention, it is possible to manufacture melting tanks and the like with less accumulation of damage due to processing, and cracking and breakage during operation can be suppressed.
[0036] In the conventional strengthened platinum alloys with dispersed oxide particles, it is difficult to increase the high-temperature strength while achieving a breaking elongation of 35% or more in a room-temperature tensile test. This breaking elongation is equal to or greater than that of a molten Pt (pure Pt) material without dispersed particles. In the present invention, the breaking elongation in a room-temperature tensile test is more preferably 40% or more. However flexible an alloy may be, there is a limit to the breaking elongation, and the upper limit of the breaking elongation is assumed to be 60% or less.
[0037] As with high-temperature creep properties, general methods are used to measure and evaluate room-temperature tensile properties. For example, the Japanese Industrial Standards stipulate JIS Z 2241 "Method of tensile testing of metallic materials." The fracture strain can be measured from the stress-strain curve obtained by room-temperature tensile testing.
[0038] (II-3) The technical significance of achieving both high-temperature creep properties and room-temperature tensile properties As described above, the strengthened platinum alloy of the present invention is a platinum alloy that has creep strength in the high temperature range as a conventional platinum alloy strengthened by dispersed particles, while having flexibility in the room temperature range. Generally, strength and flexibility are contradictory properties, and the present invention is a platinum-based material that has a good balance of physical property values related to both.
[0039] It is believed that these characteristics are manifested by the organic interaction of multiple factors, such as the dispersion of extremely fine oxides and the resulting improvement in aspect ratio, as well as the state of the atomized powder produced by the suitable oxidation treatment described below. Some of these factors may be difficult to identify. Based on these considerations, the present invention applies both high-temperature creep properties and room-temperature tensile properties as optimal methods for identifying the strengthened platinum alloy of the present invention.
[0040] (II-4) Changes in physical properties based on Zr content As described above, the strengthened platinum alloy according to the present invention has a Zr content of 0.04% by mass or more and 0.25% by mass or less. By adjusting the Zr content within this range, the strengthened platinum alloy according to the present invention can obtain other physical properties or further improve the high-temperature creep properties while maintaining the above-mentioned high-temperature creep properties and room-temperature tensile elongation.
[0041] Strengthened platinum alloys with a Zr content of 0.04% by mass or more and 0.12% by mass or less can obtain flexibility at high temperatures in addition to flexibility at room temperature. Specifically, flexibility at high temperatures refers to an increase in creep strain rate. Creep strain rate is the rate of deformation (strain) over time (dε / dt) when a material undergoes creep deformation. Creep strain rate is related to the ability to absorb thermal stress and convert it into deformation, and is an index that can also be called the stress relaxation rate. By using a material with a high creep strain rate and easy stress relaxation, cracking and fracture due to thermal stress can be suppressed.
[0042] In the strengthened platinum alloy according to the present invention, when the Zr content is set to 0.04 mass% or more and 0.12 mass% or less, the creep strain rate in a high-temperature creep test at 1400°C and a stress of 20 MPa is 1×10 -5 % / sec or more. More preferably, it is 3×10 -5% / sec or more. In this way, by increasing the creep strain rate, it is possible to obtain a strengthened platinum alloy that is further prevented from cracking or breaking due to thermal stress in the high temperature range. In particular, this regulation of creep strain rate is useful when the alloy is subjected to repeated thermal stress, and is expected to improve resistance to thermal fatigue. The upper limit of this creep strain rate is 1×10 -3 It is preferable to set the creep strain rate at % / sec or less. If the creep strain rate is too high, it may exceed the thermal stress absorption, and high temperature deformation may occur instead of normal creep deformation.
[0043] On the other hand, in the present invention, a strengthened platinum alloy with a Zr content of more than 0.12% by mass and not more than 0.25% by mass can have a higher high-temperature creep strength. In the present invention, it is assumed that the creep rupture time in a high-temperature creep test at 1400°C and a stress of 10 MPa is 100 hours or more, but by increasing the Zr content to more than 0.12% by mass, the creep rupture time is increased beyond this prerequisite. Specifically, a rupture time of 500 hours or more can be obtained under a load of 10 MPa.
[0044] However, for the strengthened platinum alloy of the present invention having a Zr content of more than 0.12% by mass and not more than 0.25% by mass, the load (stress) that is the criterion for the high-temperature creep properties (creep rupture time) is preferably 20 MPa. This is because when calculating the rupture time of a strengthened platinum alloy with high high-temperature creep properties based on a creep curve, if the stress is 10 MPa, the value may become too large and accurate judgment may not be possible. The high-temperature creep properties of the strengthened platinum alloy of the present invention having a Zr content of more than 0.12% by mass and not more than 0.25% by mass are preferably such that the creep rupture time is 20 hours or more in a high-temperature creep test at 1400°C and a stress of 20 MPa. Thus, the strengthened platinum alloy of the present invention having an increased Zr content has flexibility and is particularly excellent in high-temperature creep properties. This strengthened platinum alloy is useful in glass manufacturing equipment in which strain accumulation due to processing is not a major consideration and in equipment and members in which high-temperature creep strength is a priority.
[0045] As described above, the strengthened platinum alloys according to the present invention have different physical properties depending on the Zr content, but all of them maintain the prerequisite high-temperature creep properties and flexibility. That is, all of the strengthened platinum alloys have a creep rupture time of 100 hours or more in a high-temperature creep test at 1400°C and a stress of 10 MPa, and a rupture elongation of 35% or more in a room-temperature tensile test. More suitable values of creep rupture time in each Zr content range are 200 hours or more at a stress of 10 MPa for strengthened platinum alloys with a Zr content of 0.04% by mass or more and 0.12% by mass or less, and the upper limit is preferably 2000 hours or less. Moreover, the creep rupture time of strengthened platinum alloys with a Zr content of more than 0.12% by mass and 0.25% by mass or less is preferably 30 hours or more at a stress of 20 MPa, and the upper limit is preferably 200 hours or less.
[0046] (III) Method for producing the strengthened platinum alloy according to the present invention Next, a method for producing the strengthened platinum alloy according to the present invention will be described. The method for producing the strengthened platinum alloy according to the present invention basically follows the powder metallurgy method, which is a conventional technique. In the powder metallurgy method, first, platinum alloy powder is produced from a platinum alloy that becomes a master alloy. The platinum alloy powder is then oxidized to produce an alloy powder in which oxides are dispersed, which is then molded and subjected to appropriate processing steps, and then annealed to produce a strengthened platinum alloy with the desired shape and physical properties (high temperature creep properties, room temperature tensile properties). In the conventional manufacturing process, improvements have been made, such as adding wet grinding (ball mill grinding) and subsequent degassing treatment before the oxidation treatment of the platinum alloy powder (Patent Documents 4 and 5).
[0047] As described above, in the present invention, the improvement of high-temperature creep strength is the top priority for conventional strengthened platinum alloys, and the improvement of flexibility rather than strength is the subject of the study. From this viewpoint, the manufacturing method of the strengthened platinum alloy has been reviewed, and the oxidation treatment has been improved. That is, the manufacturing method of the strengthened platinum alloy according to the present invention includes a step of manufacturing a platinum alloy powder of a platinum alloy that essentially contains 0.04 mass% to 0.25 mass% Zr as an additive element and the balance is Pt or Pt and Rh and unavoidable impurities, a step of heating the platinum alloy powder at 800°C to 1400°C to perform an oxidation treatment, a step of molding the platinum alloy powder after the oxidation treatment, and a step of annealing the molded platinum alloy ingot, and the oxidation treatment is a step of heating the platinum alloy powder in a treatment atmosphere with an oxygen content of 50% to 100% in a naturally placed state.
[0048] (III-1) Manufacturing of platinum alloy powder In the present invention, first, a platinum alloy to be a mother alloy is obtained. The mother alloy is a platinum alloy that essentially contains 0.04 mass% or more and 0.25 mass% or less of Zr as an additive element, with the balance being Pt or Pt and Rh and unavoidable impurities. When the strengthened platinum alloy contains additive elements other than Zr (Y, Ce, etc.), the mother alloy contains these other additive elements. This platinum alloy is manufactured by a general melt casting method for precious metals.
[0049] As a method for producing platinum alloy powder from a master alloy, known metal powder production processes such as atomization and rotating electrode methods can be applied. There is also no particular limitation on the method for producing platinum alloy powder by atomization, and known atomization methods such as gas atomization and water atomization can be applied. The average particle size of the platinum alloy powder produced here is preferably 20 μm or more and 300 μm or less. This is to promote the oxidation of the additive elements in the alloy in the oxidation treatment described below.
[0050] (III-2) Oxidation treatment of platinum alloy powder The oxidation treatment is a process for oxidizing the additive elements (Zr, etc.) in the platinum alloy powder made of the platinum alloy to generate oxide particles, and is an essential process. In the present invention, the following points should be noted regarding this oxidation treatment process.
[0051] (1) Treatment state of platinum alloy powder In the present invention, the oxidation treatment requires that the platinum alloy powder is heated and oxidized in a naturally placed state. In the present invention, the naturally placed state means that platinum alloy powder in an individually independent state is placed in an oxidation treatment atmosphere without load. For example, in the degassing treatment (Patent Document 5) performed before the oxidation treatment in the above-mentioned conventional technology, the platinum alloy powder is filled into a mold and heated and sintered. In this degassing treatment, gas components adsorbed in the platinum alloy powder are desorbed, and at the same time, the platinum alloy powder is gently sintered and solidified. The powder mass of the platinum alloy powder produced by this sintering has a low density, but internal stress due to sintering remains. In addition, the platinum alloy powder particles are bonded to each other.
[0052] According to the study by the present inventors, when the platinum alloy powder having the limited content of additive elements as in the present invention is oxidized, the platinum alloy powder lump as described above does not have a suitable oxidation state, and it is not possible to manufacture a strengthened platinum alloy having the desired physical properties. This is because the processing gas (oxygen) does not easily reach each powder in the platinum alloy powder lump, but it is also considered that the load due to the internal stress in the platinum alloy powder is also related to this.
[0053] Therefore, in the present invention, the platinum alloy powder is oxidized in a naturally placed state. Operations that disturb the naturally placed state of the platinum alloy powder include the firing accompanied by sintering as described above, and also the filling of the platinum alloy powder into a mold while applying pressure during the oxidation treatment. However, the weight of the platinum alloy powder does not fall under the load referred to here. A specific method of treatment in a naturally placed state in the present invention involves loading the platinum alloy powder into a tray or container without applying pressure, and placing it in a heating furnace as is to perform heat treatment.
[0054] By the oxidation treatment in the natural state, the gas (oxygen-containing gas) in the heat treatment device is evenly distributed in the platinum alloy powder, and the oxidation of the added elements can be promoted. As a result, even trace amounts of added elements in the platinum alloy are oxidized, and an alloy powder that serves as a precursor of the strengthened platinum alloy having the unique physical properties of the present invention described above is produced. It is also presumed that the heat treatment in the natural state without load also relaxes the strain and lattice defects contained in the platinum alloy powder. The inventors consider that this also functions in producing a suitable strengthened platinum alloy.
[0055] (2) Adjustment of the oxidation treatment atmosphere In the production of the strengthened platinum alloy according to the present invention, it is essential that the atmosphere in the oxidation treatment has an oxygen content (oxygen partial pressure) of 50% or more. In the production of conventional strengthened platinum alloys, the heat treatment atmosphere is often an air atmosphere. In the present invention, since it is necessary to effectively oxidize the additive elements whose contents are limited, the oxygen content of the oxidation treatment atmosphere is strictly controlled. According to the investigations of the present inventors, when the oxidation treatment atmosphere is an air atmosphere in the production method of the present invention, there is a tendency for oxide particles to become coarse. The oxygen content of the oxidation treatment atmosphere is preferably 80% or more, and more preferably 99% or more.
[0056] Such control of the oxidation treatment atmosphere leads to stabilization of the oxidation state of the additive elements in the platinum alloy powder after the treatment, and thus to stabilization of the properties of the strengthened platinum alloy. In particular, the strengthened platinum alloy according to the present invention requires predetermined values for both physical properties at high temperature and room temperature. Control of the oxidation treatment atmosphere is effective in suppressing the variation in physical properties and producing a strengthened platinum alloy that can be used stably.
[0057] In the present invention, the oxidation treatment is performed based on the above two characteristics. The temperature of the oxidation treatment is set to 800°C or more and 1400°C or less. If the temperature is less than 800°C, the oxidation of Zr and the like does not progress easily. In addition, the oxidation of the added elements is promoted by increasing the treatment temperature, but the oxidation is not promoted even if the heat treatment is performed at a temperature above 1400°C, and there is a concern that the crystal grains of the oxide and the platinum alloy matrix will become coarse, so the upper limit is set to 1400°C. The treatment time is preferably set to 1 hour or more and 24 hours or less, although it depends on the amount of platinum alloy powder.
[0058] (3) Relationship with conventional manufacturing methods of strengthened platinum alloys In the conventional manufacturing method of strengthened platinum alloys described above, some improvements have been proposed before and after the oxidation treatment of platinum alloy powder in order to improve the high-temperature creep properties. For example, additional processes such as a process of wet-milling platinum alloy powder (platinum alloy powder before and after oxidation treatment) in a solvent (water, organic solvent, or a mixed solvent of water and organic solvent) using a ball mill or the like (Patent Documents 2 and 4) and a degassing process of heating the platinum alloy powder after wet milling in a vacuum (Patent Document 5) are known. These additional processes are considered to be effective in preventing the state of the oxides of the added elements and the swelling and deformation of the material during use.
[0059] In the manufacturing method of the strengthened platinum alloy according to the present invention, these wet grinding and degassing steps may be included, but are not essential. In some cases, it is preferable not to perform these additional processes. In other words, it is preferable to manufacture platinum alloy powder from the mother alloy, oxidize this as it is in a natural state, and then immediately mold it. Even with such a simplified manufacturing method, it is possible to manufacture the strengthened platinum alloy according to the present invention by performing an appropriate oxidation treatment. Reducing the number of steps not only contributes to cost reduction by reducing the number of man-hours, but also leads to stabilization of the product characteristics.
[0060] (III-3) Molding process after oxidation treatment Then, the platinum alloy powder made of the platinum alloy having the oxide particles dispersed therein by the oxidation treatment is molded to produce a platinum alloy ingot with high density. The molding process is performed to obtain a shape suitable for processing when a rolling process is performed thereafter. As a specific processing method in the molding process, hot forging can be applied. The platinum alloy powder is often turned into a powder lump by sintering due to heating caused by the above-mentioned oxidation treatment. In the hot processing, the platinum alloy powder lump is preferably heated to 1000°C or more and 1400°C or less for processing. It is preferable that the hot forging is performed multiple times, with heating and forging being one set.
[0061] As a specific processing method for the molding process, a hot pressing method in which compression processing and sintering are carried out simultaneously can also be applied. In the case of hot pressing, the conditions are preferably 1000° C. to 1400° C. and a pressure of 10 MPa or more.
[0062] The platinum alloy powder before the molding process may be preliminarily heated and pre-sintered after the oxidation treatment, but pre-sintering is not essential because the platinum alloy powder can be sintered by the oxidation treatment.
[0063] (III-4) Post-processing (rolling, etc.) The strengthened platinum alloy after forming can be subjected to post-processing steps such as rolling as necessary to produce a strengthened platinum alloy plate material, etc. Furthermore, in order to form the alloy into a shape according to the application (the glass manufacturing device to which it is applied), further processing steps such as rolling, extrusion, and drawing can be added. These post-processing steps may involve repeating the same processing process multiple times, or may involve a combination of different processing processes. Furthermore, when performing multiple processing steps, intermediate heat treatment may be performed in consideration of work hardening.
[0064] (III-5) Annealing process After the above forming process and after any necessary post-processing process, the strengthened platinum alloy is heat-treated (annealed). This is to obtain a suitable material structure by developing a recrystallized structure by annealing. The conditions of the annealing process are preferably a heating temperature of 1000°C to 1500°C and a treatment time of 0.5 hours to 3 hours. The annealing process can be carried out in the air, but may also be carried out in a non-oxidizing atmosphere.
[0065] (IV) Uses of the strengthened platinum alloy according to the present invention The strengthened platinum alloy according to the present invention is suitable as a constituent material for various devices used in high-temperature environments. In particular, the present invention is useful as a constituent member of a glass manufacturing device for manufacturing various glass materials. The glass manufacturing device according to the present invention includes a melting tank, a fining tank, a stirring tank, and the like, as towers and tanks capable of storing molten glass. In addition, a stirrer (stirring rod) for stirring molten glass in a stirring tank to perform homogenization processing is also a target. Furthermore, a device for forming molten glass and a bushing (nozzle and base plate) for spinning are also a target. Particularly preferred are towers and tanks such as melting tanks that may be partially subjected to strong processing during manufacturing. However, regardless of the presence or absence of processing during manufacturing and the strength of the processing, the present invention can be widely used as a constituent material for various glass manufacturing devices. Therefore, the present invention is also applicable to a trough-shaped flow path, a throat, a connecting pipe, and the like for circulating molten glass. In addition to applications other than glass manufacturing equipment, the strengthened platinum alloy according to the present invention is also useful as a constituent material for crucibles used in single crystal growth and the like. Effect of the Invention
[0066] The strengthened platinum alloy according to the present invention described above exhibits good values for both high-temperature creep properties in the high-temperature range and room-temperature tensile properties in the room-temperature range. Therefore, it has appropriate high-temperature strength and flexibility. According to the present invention, it is possible to suppress the occurrence and propagation of cracks that were observed when conventional strengthened platinum alloys were applied. Therefore, the present invention can contribute to the stable operation of glass manufacturing equipment, particularly a melting tank for molten glass. [Brief description of the drawings]
[0067] [Figure 1] 4 is a SEM photograph of the surface of platinum alloy powder after oxidation treatment according to the first embodiment and a comparative example. [Diagram 2] 1 shows the results of observation of the cross-sectional structure of the strengthened platinum alloy of the first embodiment and a comparative example. [Diagram 3] FIG. 2 is a graph showing creep rupture curves at 1400° C. of the strengthened platinum alloy of the first embodiment (0.07% Zr) and the comparative example (0.3% Zr). [Figure 4] FIG. 2 is a graph showing creep strain rates at 1400° C. of the strengthened platinum alloy of the first embodiment (0.07% Zr) and the comparative example (0.3% Zr). [Diagram 5] FIG. 2 is a diagram showing stress-strain curves in room temperature tensile tests of the strengthened platinum alloys of the first embodiment (0.07% Zr) and the comparative example (0.3% Zr) after annealing at 1400° C. [Figure 6] 4 is a cross-sectional photograph of the strengthened platinum alloy of the first embodiment and the strengthened platinum alloy of the comparative example after a thermal fatigue test. [Figure 7] 13 shows creep curves of various strengthened platinum alloys (Zr content: 0.01 to 0.3 mass%) according to the second embodiment. [Figure 8] FIG. 11 is a graph showing the measurement results of the oxygen content and the theoretical oxygen content of the strengthened platinum alloy (Zr content: 0.01% to 0.3%) according to the second embodiment. [Figure 9] Creep curves of the strengthened platinum alloys (Pt-Zr-Y and Pt-Y) of the third embodiment DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0068] First embodiment A preferred embodiment of the present invention will be described below. In this embodiment, a strengthened platinum alloy containing 0.07 mass% Zr as an additive element was manufactured, and its high temperature creep properties and room temperature tensile properties were evaluated. For comparison, a conventional strengthened platinum alloy (Zr content: 0.3 mass%) was manufactured and similar evaluation was performed.
[0069] [Production of platinum alloy powder (atomized powder)] First, 50.0 g of a button-shaped Pt-12 mass% Zr alloy was prepared as a mother alloy by vacuum arc melting. This mother alloy and pure Pt were cast by vacuum melting to produce a platinum alloy rod (dimensions: φ44 mm × 260 mm) of Pt-0.07 mass% Zr. Then, an electrode induction melting gas atomizing device using this rod as an electrode produced an atomized powder of a platinum alloy (Pt-0.07 mass% Zr alloy). The particle size of the atomized powder of the platinum alloy produced at this time was 300 μm or less, and all of the produced atomized powder was collected and used for the subsequent process.
[0070] [Oxidation treatment] The produced atomized powder was put directly into a heat treatment vessel from the recovery vessel of the atomizing device without applying any particular pressure. Then, in this natural state, it was subjected to heat treatment for oxidation treatment. The oxidation treatment was performed by heating at 1300°C for 6 hours in a pure oxygen atmosphere to produce atomized powder made of Pt alloy with Zr oxide particles dispersed therein. The heating caused by this oxidation treatment sintered the platinum alloy powder into a powder lump.
[0071] [Forming and rolling processes] The platinum alloy powder lump obtained by the above oxidation treatment was taken out of the heat treatment vessel and subjected to forming processing by hot forging. In the hot forging processing, the platinum alloy powder lump was heated to 1300°C and forged. Six sets of forging processing were performed. After the forming processing step, cold rolling processing was performed to produce a platinum alloy plate material with a thickness of 1 mm. During the cold rolling process, intermediate heat treatment (annealing treatment at 1250°C in air for 30 minutes) was performed and the plate material was obtained by rolling multiple times. After rolling processing, the platinum alloy plate material was annealed at 1400°C for 1 hour to produce a reinforced platinum alloy plate material.
[0072] Comparative Example A button-shaped Pt-15 mass% Zr alloy (165 g) was prepared as a mother alloy by vacuum arc melting. This mother alloy and pure Pt were processed into a platinum alloy rod (dimensions: φ44 mm × 260 mm) of Pt-0.3 mass% Zr by vacuum melting. Then, atomized powder of the Pt-Zr alloy was produced in the same manner as in the first embodiment.
[0073] [Wet grinding and degassing] In this comparative example, the atomized powder was subjected to wet pulverization and degassing treatment, followed by oxidation treatment. The atomized powder and Pt-ZrO2 alloy balls with a diameter of 5 mm were placed in an attritor pot (made of Pt-ZrO2 alloy), which is a wet pulverizer. After sealing the pot, an organic solvent (heptane) was introduced. Then, the pulverizer blade was rotated at a rotation speed of 215 rpm, and wet fine pulverization treatment was performed for about 5 hours. The platinum alloy fine powder after pulverization was dried at 120°C for 7 hours to remove the organic solvent.
[0074] The platinum alloy powder after wet milling was packed into an open carbon container (120 mm x 120 mm, depth 150 mm) and placed in a gas atmosphere furnace where it was heated and held at 1300°C for 3 hours under an argon atmosphere at atmospheric pressure for degassing treatment. As a result of the degassing treatment, the platinum alloy powder was in the form of powder lumps that did not easily crumble.
[0075] [Oxidation treatment, molding and rolling processing] The platinum alloy powder lump solidified in the carbon container by the degassing process was subjected to an oxidation process. In this oxidation process, the platinum alloy powder lump was heated in an air atmosphere at 1300°C for 1 hour. Thereafter, the platinum alloy powder lump was subjected to hot forging and rolling in the same manner as in the first embodiment, and further subjected to an annealing process to produce a reinforced platinum alloy plate material.
[0076] Comparative observation and testing [Microstructures of platinum alloy powder and reinforced platinum alloy after oxidation treatment] FIG. 1 is an SEM photograph (magnification 10,000 times) of the surface of platinum alloy powder (platinum alloy powder lump) after oxidation treatment in the manufacturing process of the strengthened platinum alloy of this embodiment and the comparative example. In the platinum alloy powder of the comparative example, it can be seen that rounded oxide particles (ZrO2) are connected. In the platinum alloy powder of this embodiment, fine oxide particles are dispersed in an isolated state. This difference in particle size and distribution state of the oxide particles is considered to be due to the fact that the Zr content (0.30 mass%) of the comparative example is higher than the Zr content (0.07 mass%) of this embodiment. However, these platinum alloy powders differ in the surface morphology of the platinum matrix. In the platinum alloy powder after oxidation treatment of this embodiment, steps due to surface undulations that are presumed to be the exposure of the sliding surface are seen. On the other hand, there is no such morphological change in the matrix of the platinum alloy powder after oxidation treatment of the comparative example. The present inventors presume that this is due to the influence of strain and residual stress introduced during degassing treatment and wet grinding in the manufacturing process of the comparative example. It is not clear how this difference in matrix morphology affects the properties of the strengthened platinum alloy after molding and annealing. However, considering the cross-sectional structure of the strengthened platinum alloy and the results of high-temperature creep properties and room-temperature tensile properties described below, it is considered that the above differences in the platinum alloy powder after oxidation treatment have some effect.
[0077] FIG. 2 shows the results of observing the cross-sectional structure of the strengthened platinum alloy of this embodiment and the comparative example. In both strengthened platinum alloys, a material structure is exhibited in which leaf-shaped crystal grains with a large aspect ratio are alternately stacked. It is believed that there is no clear difference in the cross-sectional structure between the strengthened platinum alloy of this embodiment and the strengthened platinum alloy of the comparative example. The inventors believe that this cross-sectional structure of the strengthened platinum alloy of this embodiment contributes to ensuring high-temperature strength.
[0078] [High temperature creep test / room temperature tensile test] A high-temperature creep test was carried out on the strengthened platinum alloy of the first embodiment and the comparative example manufactured above. Test pieces (JIS 13B tensile test pieces) for creep tests and room temperature tensile tests were processed and collected from the plate material of the strengthened platinum alloy manufactured above. The test temperature was 1400°C, and a stress rupture (creep) test was carried out at a constant load. In this embodiment, a plurality of loads (stresses) were set, and a high-temperature creep test was carried out at each set load. For the strengthened platinum alloy of this embodiment, the rupture time was measured at each load of 8, 10, 12, 15, 20, and 25 MPa (n=2). In addition, for the strengthened platinum alloy of the comparative example, the creep test was carried out at 15, 20, and 25 MPa to measure the rupture time (n=2). In addition, considering that the Zr content of the strengthened platinum alloy of the comparative example is relatively large, the load of the comparative example is set to be relatively high. Then, the rupture time at each load was plotted, and a creep curve was created by power approximation using spreadsheet software (Microsoft Excel 2010).
[0079] Further, a room temperature tensile test (n=2) was carried out on the strengthened platinum alloys of the first embodiment and the comparative example. In the room temperature tensile test, a stress-strain curve was created and the fracture elongation was measured.
[0080] FIG. 3 shows creep rupture curves (stress-rupture time) at 1400°C for the strengthened platinum alloys of the first embodiment and the comparative example. The creep rupture time at a stress of 10 MPa was 275 hours (average of actual measurements) for the first embodiment and 250 hours (average of actual measurements) for the comparative example. The strengthened platinum alloy of the first embodiment was confirmed to have sufficient high-temperature strength in terms of high-temperature creep properties (10 MPa), as the rupture time was slightly longer than that of the comparative example. When compared at a stress of 20 MPa, the comparative example had a higher high-temperature creep strength.
[0081] 4 is a diagram showing the creep strain rate at 1400° C. of the strengthened platinum alloys of the first embodiment and the comparative example. From FIG. 4, it can be seen that the creep strain rate of the strengthened platinum alloy of the first embodiment at a stress of 20 MPa is 6.83×10 -5 % / sec (average value), whereas the creep strain rate of the comparative strengthened platinum alloy was 5.94×10-6 % / sec (average value). It is clear that the strengthened platinum alloy of the first embodiment has a clearly higher creep strain rate than the comparative example.
[0082] FIG. 5 shows the results (stress-strain curves) of room temperature tensile tests of the strengthened platinum alloys of the first embodiment and the comparative example. FIG. 5 shows the room temperature tensile properties (n=2) of pure platinum (99.9% Pt) by melt casting under the same conditions as the reference example. From FIG. 5, the fracture elongation at the time of material fracture is 37.2% (average value) for the strengthened platinum alloy of the present embodiment, 29.4% (average value) for the strengthened platinum alloy of the comparative example, and 37.8% (average value) for the pure platinum (99.9% Pt) melt material. The strengthened platinum alloy of the present embodiment shows a fracture elongation equivalent to that of the reference example melt material. Therefore, it was confirmed that the strengthened platinum alloy according to the present invention has the same flexibility as the pure platinum melt material, even though it is an alloy (oxide dispersion type alloy).
[0083] From the results of the high-temperature creep test and the room-temperature tensile test, it was confirmed that the strengthened platinum alloy of this embodiment has sufficient high-temperature creep strength comparable to that of the conventional strengthened platinum alloy (comparative example), and is also excellent in elongation (flexibility) at room temperature. It was also confirmed that the strengthened platinum of this embodiment (Zr content 0.07 mass%) has a high creep strain rate at 1400°C under a stress of 20 MPa.
[0084] [Thermal fatigue test] A thermal fatigue test was conducted on the strengthened platinum alloys of the present embodiment and the comparative example, simulating the use of a melting tank, which is a glass manufacturing apparatus. A plate material of 300 mm (L) x 100 mm (W) was cut out from the plate material produced above to prepare a test material. In the thermal fatigue test, first, electrodes for electrical heating are attached to both ends of the test material, and the test material is heated to a predetermined test temperature. Air is blown onto the center of the heated test material for a certain period of time to locally cool it. As a result, only the center portion of the test material that has expanded due to heating shrinks, generating thermal stress. Then, after the air blowing, air is blown again after a certain period of time has elapsed. This heating-cooling cycle is repeated, and the presence or absence of cracks is confirmed to evaluate the resistance to thermal fatigue. In the thermal fatigue test of the present embodiment, in detail, the test material was conducted under the following conditions. Test temperature: 1400℃ ·Electricity conditions: 5V / 1350A Air spray conditions: 6L / 3 seconds Cycle conditions: 20 seconds / 1 cycle
[0085] In the thermal fatigue test, under the above conditions, at the stage of 2000 or 5000 cycles, a penetrant test (PT test) was performed on the surface (air-blasted surface) of the test material, and both the front and back were observed to confirm the presence or absence of penetrating cracks.
[0086] As a result of the above thermal fatigue test, in the strengthened platinum alloy of the comparative example, a through crack occurred at the stage of 2000 cycles. On the other hand, in the strengthened platinum of the present embodiment, no through crack occurred even at the cycle number of 5000. Even when the test of the test material of the present embodiment was extended to 8000 cycles, no crack occurred. Figure 6 is a photograph of the cross section of the strengthened platinum alloy of the present embodiment (after 2000 cycles) and the strengthened platinum alloy of the comparative example (after 2000 cycles) after the thermal fatigue test.
[0087] From the results of this thermal fatigue test, it was confirmed that the strengthened platinum alloy of this embodiment has resistance to thermal fatigue four times or more times that of the comparative example in terms of the number of cycles. Such evaluation results are believed to be due to the flexibility confirmed by the room temperature tensile properties.
[0088] Second embodiment In this embodiment, strengthened platinum alloys were manufactured with the Zr content adjusted to 0.01 mass%, 0.04 mass%, 0.10 mass%, 0.14 mass%, 0.21 mass%, and 0.30 mass%. The manufacturing process of the strengthened platinum alloy in this embodiment is the same as that in the first embodiment. That is, a platinum alloy bar containing a predetermined amount of additive elements was manufactured to produce atomized powder, and then the rod was oxidized in a pure oxygen atmosphere in a natural placement state. After that, the plate of the strengthened platinum alloy was manufactured by hot forging, rolling, and annealing.
[0089] Then, high-temperature creep tests and room-temperature tensile tests were conducted on each strengthened platinum alloy, and the physical properties were confirmed. In the high-temperature creep tests, similar to the first embodiment, multiple loads (stresses) were set. Here, too, the loads were set in consideration of the Zr content of the strengthened platinum alloy. For the strengthened platinum alloy with a Zr content of 0.01% by mass, tests were conducted at 7, 10, and 15 MPa. For the strengthened platinum alloy with a Zr content of 0.04 mass%, tests were performed at 10, 12, and 15 MPa. For the strengthened platinum alloy with a Zr content of 0.1 mass% or more, tests were performed at 15, 20, and 25 MPa. The room temperature tensile test method was the same as in the first embodiment. Furthermore, in this embodiment, the same thermal fatigue test (5000 cycles) as in the first embodiment was performed.
[0090] FIG. 7 shows creep curves for the strengthened platinum alloys (Zr contents: 0.01 mass%, 0.04 mass%, 0.10 mass%, 0.14 mass%, 0.21 mass%, and 0.30 mass%) produced in this embodiment. The creep rupture times at stresses of 10 MPa and 20 MPa were determined based on these creep curves. The results, as well as the room temperature rupture elongation, creep strain rate (stress of 20 MPa), and results of the thermal fatigue test (presence or absence of through cracks) are shown in Table 1. In Table 1, the creep rupture times of each strengthened platinum alloy (10 MPa, 20 MPa) are given priority as actual measured values (average values), and when actual measured values were not available, they were calculated from the creep curves (FIG. 7).
[0091] [Table 1]
[0092] Referring to Table 1, the strengthened platinum alloys with a Zr content of 0.04 mass% or more have a rupture time (10 MPa) of more than 100 hours in a high-temperature creep test (1400°C). Although the high-temperature strength of these strengthened platinum alloys is lower than that of the conventional strengthened platinum alloy (No. 8: Comparative Example), it can be said that they exhibit sufficient high-temperature strength. However, the strengthened platinum alloy (No. 1) with a Zr content of 0.01 mass% had a short creep rupture time of 20 hours and was inferior in high-temperature strength. In addition, this strengthened platinum alloy No. 1 exhibited high-temperature deformation behavior, and it was not possible to calculate the deformation rate as a creep strain rate. Therefore, it was confirmed that even if the Zr content is limited to 0.04 mass% or less, it is not preferable to limit the Zr content.
[0093] On the other hand, looking at the fracture elongation in room temperature tensile tests, the strengthened platinum alloy with a Zr content of 0.01 mass% had the largest fracture elongation, but all of the strengthened platinum alloys with a Zr content of 0.04 mass% or more showed 35% or more. There is little difference in the fracture elongation at room temperature due to the Zr content. And these strengthened platinum alloys have clearly larger fracture elongation at room temperature than the comparative examples.
[0094] The creep rupture time (10 MPa) increases with increasing Zr content. However, when the Zr content is 0.3 mass% (No. 7), the creep rupture time drops significantly in contrast to this trend. The creep rupture time in this case also exceeds 100 hours, and it cannot be said that the high-temperature strength is inferior. However, considering the tendency for strength to decrease and the risk of weldability deterioration when the amount of added elements is increased as described above, it is appropriate to assume that the upper limit of the Zr content is 0.25 mass%.
[0095] In addition, when looking at both the creep rupture time and high-temperature creep strain rate of the strengthened platinum alloys (No. 2 to No. 6) with Zr contents of 0.04% to 0.21% by mass, the strengthened platinum alloys (No. 2 to No. 4) with low Zr contents (0.04% to 0.1% by mass) have particularly high high-temperature creep strain rates. On the other hand, the strengthened platinum alloys with high Zr contents (0.14% to 0.21% by mass) have further improved high-temperature creep strength, with creep rupture times of 20 hours or more at a stress of 20 MP. It can be said that the high-Zr strengthened platinum alloys do not have particularly high high-temperature creep strain rates (although they are higher than the comparative examples). These results indicate that the strengthened platinum alloys of the present invention have physical properties that change depending on the Zr content. In addition, estimating from the trends of both the rupture time (10 MPa) and creep strain rate in this embodiment, when classifying the strengthened platinum alloy of the present invention based on the above-mentioned differences in physical properties, the boundary should be 0.12 mass %.
[0096] However, all of the strengthened platinum alloys have sufficient high-temperature creep strength and room-temperature tensile elongation (flexibility). As a result, the strengthened platinum alloys specified in the present invention did not crack in thermal fatigue tests. Therefore, the Zr content can be set in consideration of the required properties depending on the application, etc.
[0097] [Oxygen content measurement] Here, the oxygen content was measured for the strengthened platinum alloys manufactured in the second embodiment that contained only Zr as an additive element (Zr concentration: 0.01 mass%, 0.04 mass%, 0.07 mass%, 0.10 mass%, 0.14 mass%, 0.21 mass%, 0.30 mass%). The oxygen content was measured using an oxygen / nitrogen analyzer (EMGA-920, manufactured by Horiba, Ltd.). The actual oxygen content was measured and the theoretical oxygen content of each alloy was calculated. The theoretical oxygen content was calculated under the assumption that all Zr in the alloy was formed into ZrO2.
[0098] Fig. 8 is a diagram showing the measurement results of the oxygen content and the theoretical oxygen content of each strengthened platinum alloy. From Fig. 8, it can be seen that the oxygen content in each strengthened platinum alloy exceeds the theoretical oxygen content. The actual oxygen content of each strengthened platinum alloy is 1.0 to 1.5 times the theoretical oxygen content. This oxygen content that is greater than the theoretical oxygen content is thought to include an increase due to the oxidation of unavoidable impurities, but even taking this into consideration, it can be said that the strengthened platinum alloy produced in this embodiment is in a state in which the added element (Zr) is highly oxidized.
[0099] Here, the oxygen content was measured in the same manner for the comparative example of the first embodiment (Zr concentration: 0.3 mass%), and was found to be 1090 to 1140 ppm. The strengthened platinum alloy of this comparative example also contains oxygen that is 1.03 to 1.08 times the theoretical oxygen content or more. The ratio of the oxygen content is higher in the strengthened platinum alloy of this embodiment, but the difference is not so obvious. Nevertheless, in this embodiment, there is a clear difference in the physical property value (breaking elongation) in room temperature tensile testing and the results of thermal fatigue testing. This is considered to be due to the fact that the strengthened platinum alloy of this embodiment has improved characteristics due to factors different from those of the conventional considerations regarding the amount and grain size of oxides. In the present invention, both high temperature creep properties and room temperature tensile properties are applied to identify this.
[0100] Third embodiment In this embodiment, the influence of the addition of an additive element other than Zr was examined. Specifically, two types of strengthened platinum alloys were manufactured: a strengthened platinum alloy containing Y as an additive element together with Zr (total content of additive elements: 0.07% by mass), and a strengthened platinum alloy containing only Y as an additive element instead of Zr (Y content: 0.07% by mass). The manufacture of these strengthened platinum alloys was also similar to that of the first and second embodiments.
[0101] Then, a high-temperature creep test and a room-temperature tensile test were performed on each of the strengthened platinum alloys to confirm their physical properties. The methods of the high-temperature creep test and the room-temperature tensile test were the same as those in the first embodiment.
[0102] Fig. 9 shows creep curves of the strengthened platinum alloy (No. 9) containing 0.06 mass% Zr + 0.01 mass% Y and the strengthened platinum alloy (No. 10) containing 0.07 mass% Y, both manufactured in this embodiment. The creep rupture time at a stress of 10 MPa was calculated based on the creep curves. The results, room temperature rupture elongation, and creep strain rate (stress of 20 MPa) are shown in Table 2.
[0103] [Table 2]
[0104] From Table 2, the strengthened platinum alloy (No. 10) containing only Y as an additive element without Zr had a creep rupture time exceeding 100 hours, so that the high-temperature strength was satisfactory, but the room-temperature rupture elongation was 15% lower than that of the first embodiment (No. 3). With this alloy, there is concern about the accumulation of strain during room-temperature processing. On the other hand, even when Y is added, the strengthened platinum alloy (No. 9) containing both Zr and Y has high high-temperature creep properties equivalent to those of the first embodiment (No. 3), and the room-temperature elongation is 35% or more, which is sufficiently high. From these results, Zr should be said to be an essential additive element in order to secure both high-temperature strength and flexibility, and it is considered that the addition of Y alone is not preferable.
[0105] Therefore, the same thermal fatigue test as in the first embodiment was carried out on the strengthened platinum alloy No. 9 containing Zr and Y as additive elements, which cleared the criteria of the present invention in terms of high temperature strength and room temperature elongation in the above tests, and this strengthened platinum also did not experience any through cracks after 5000 cycles. From this result, it was confirmed that the strengthened platinum alloy of the present invention can be added with other elements in addition to Zr.
[0106] The strengthened platinum alloy (No. 10) containing only Y as an additive element without Zr had a higher creep strain rate at 1200°C than the comparative example. This is presumably because the oxidation state of the additive elements was favorable due to the manufacturing process in this embodiment. [Industrial Applicability]
[0107] The present invention is a strengthened platinum alloy that has tensile properties and flexibility at room temperature while maintaining high-temperature creep properties at high temperatures. According to the present invention, it is possible to effectively suppress through cracks at the bottom of glass equipment such as molten glass melting tanks that are manufactured by subjecting the equipment to severe processing, thereby extending the operating life of the equipment. According to the present invention, it is possible to achieve stable production and supply of glass materials when manufacturing various glass materials such as optical glass and glass fiber.
Claims
1. A strengthened platinum alloy comprising a matrix of a PtRh alloy having a Pt or Rh content of 5% by mass or more and 40% by mass or less, in which dispersed particles of an oxide of an additive element are dispersed, and the platinum alloy powder in which the oxide is dispersed is molded, The strengthened platinum alloy essentially contains 0.04 mass% or more and 0.25 mass% or less of Zr as the additional element, with the balance being composed of the constituent metals of the matrix, oxygen, and inevitable impurities; The creep rupture time in a high-temperature creep test at 1400°C and a stress of 10 MPa is 100 hours or more; The strengthened platinum alloy is characterized in that the breaking elongation in a room temperature tensile test is 35% or more.
2. Contains 0.04 mass% or more and 0.12 mass% or less of Zr as an additive element, The creep strain rate in a high-temperature creep test at 1400°C and a stress of 20 MPa was 3×10 -5 % / sec or more 3×10 -4 2. The strengthened platinum alloy of claim 1, wherein the strengthening coefficient is less than 1.0% / sec.
3. Contains Zr in an amount of more than 0.12 mass% and not more than 0.25 mass% as an additive element, 2. The strengthened platinum alloy according to claim 1, which has a creep rupture time of 20 hours or more in a high temperature creep test at 1400° C. and a stress of 20 MPa.
4. The strengthened platinum alloy according to any one of claims 1 to 3, further comprising at least one of Y, Ce, Sc, and Hf as an additive element, and the total content of the additive elements is 0.04 mass% or more and 0.25 mass% or less.
5. The strengthened platinum alloy according to any one of claims 1 to 4, wherein the oxygen content of the strengthened platinum alloy is 1.0 to 2.0 times the theoretical oxygen content resulting from oxides of the added elements.
6. A method for producing a strengthened platinum alloy according to any one of claims 1 to 5, comprising the steps of: A step of producing a platinum alloy powder essentially containing 0.04 mass% or more and 0.25 mass% or less of Zr as an additive element, with the balance being Pt or Pt and Rh, and unavoidable impurities; A step of heating the platinum alloy powder at 800° C. or more and 1400° C. or less to perform an oxidation treatment; A step of molding the platinum alloy powder after the oxidation treatment; Annealing the formed platinum alloy ingot; The oxidation treatment is a process for producing a strengthened platinum alloy, in which the platinum alloy powder produced in the process for producing the platinum alloy powder is heated in a treatment atmosphere having an oxygen content of 50% or more and 100% or less in a natural, unloaded state without being subjected to a crushing treatment.
7. A glass manufacturing apparatus comprising the strengthened platinum alloy according to any one of claims 1 to 5.
Citation Information
Patent Citations
Oxide dispersion enhanced platinum or plating alloy and its production
JP1994336631A
Production of strengthened platinum material
JP1996134511A
Dispersively solidified platinum material, production of the material and use of the material
JP1998280070A
Strengthened platinum material and its production
JP2000160268A
Method for producing oxide-dispersed alloy
JP2006057164A