Magnetic sensor and method for manufacturing the same

The FeSiAl alloy thin film, with specific composition and production methods, addresses sensitivity limitations in magnetic sensors by providing improved soft magnetic properties and cost-effectiveness, leading to a high-performance magnetic sensor configuration.

JP7577274B2Active Publication Date: 2024-11-05TOHOKU UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020207446
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-15
Publication Date
2024-11-05
Estimated Expiration
2040-12-15

AI Technical Summary

Technical Problem

Existing magnetic sensors, such as those using NiFe, CoFeB, and CoFeSiB alloys for their free layers, face limitations in sensitivity due to the magnetocrystalline anisotropy constant and saturation magnetization, necessitating the development of alternative alloys with better soft magnetic properties.

Method used

The use of an FeSiAl alloy thin film with specific compositions (7-10 wt% Si, 4-8 wt% Al, balance Fe) and a film thickness of 20-100 nm, produced through sputtering and heat treatment at 350-500°C, enhances the soft magnetic properties of the free layer in magnetic tunnel junction (MTJ) elements.

Benefits of technology

The FeSiAl alloy thin film achieves improved sensitivity and lower manufacturing costs compared to conventional alloys, resulting in a magnetic sensor with enhanced performance and new configuration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577274000002
    Figure 0007577274000002
  • Figure 0007577274000003
    Figure 0007577274000003
  • Figure 0007577274000004
    Figure 0007577274000004
Patent Text Reader

Abstract

To provide: an FeSiAl alloy thin film having good soft magnetic characteristics and capable of being used for a free layer of an MTJ element, and a method for producing an FeSiAl alloy thin film; and a magnetic sensor in which an FeSiAl alloy thin film is included in the free layer of an MTJ element and a method for manufacturing a magnetic sensor.SOLUTION: An FeSiAl alloy thin film contains 7-10 wt.% of Si and 4-8 wt.% of Al, with the balance being Fe and inevitable impurities, and has a film thickness of 20-100 nm. A magnetic sensor uses a magnetic tunnel junction element having a fixed layer with a fixed magnetization direction, a free layer with a magnetization direction that can be changed, and an insulation layer disposed between the fixed layer and the free layer, the free layer including an FeSiAl alloy thin film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention , magnetic The present invention relates to a magnetic sensor and a method for manufacturing the magnetic sensor. [Background technology]

[0002] A highly sensitive magnetic sensor is a TMR sensor that utilizes the tunnel magnetoresistance (TMR) effect of a magnetic tunnel junction (MTJ) element. The MTJ element has a fixed layer whose magnetization direction is fixed, a free layer whose magnetization direction is variable, and an insulating layer disposed between the fixed layer and the free layer. The characteristics of the magnetic sensor can be controlled by controlling the magnetic anisotropy of the free layer. Such a magnetic sensor can detect weak magnetic fields generated from living organisms such as the heart and brain, and can be used in biomagnetic measurement devices that operate at room temperature. In addition, it can measure current without contact, consumes little power, and has high sensitivity, so it can be effectively used, for example, to detect the remaining charge of the battery of an electric vehicle. In addition, it can be used as a magnetic sensor for non-destructive testing to detect breakage or deterioration of reinforcing bars in concrete structures.

[0003] Conventionally, MTJ elements that can be used in magnetic sensors include those that use a NiFe alloy for the free layer (see, for example, Non-Patent Document 1), those that use a CoFeB alloy (see, for example, Non-Patent Document 2), and those that use a CoFeSiB alloy (see, for example, Non-Patent Document 3).

[0004] Here, the sensitivity of the magnetic sensor is determined by the magnetoresistance ratio of the free layer of the MTJ element, the TMR ratio, and the anisotropic magnetic field, H k Then, TMR ratio / 2H k From this formula, it can be seen that the TMR ratio is large and the anisotropic magnetic field H k The smaller the value, the higher the sensitivity. In addition, the magnetocrystalline anisotropy constant K1 and the magnitude of saturation magnetization M s Then, the anisotropy magnetic field H k is H k =2×K1 / Ms Thus, the anisotropy magnetic field H k is proportional to the magnetocrystalline anisotropy constant K1, the sensitivity of the magnetic sensor increases even if the magnetocrystalline anisotropy constant K1 is reduced.

[0005] In order to increase the sensitivity compared to conventional magnetic sensors, it is considered effective to expand the scope of alloys used in the free layer to alloys that have not been used in the free layer so far, unlike the alloys described in Non-Patent Documents 1 to 3. An example of an alloy that has not been used in the free layer so far is an FeSiAl alloy (Sendust) whose main components are 6wt% to 12wt% Si, 3wt% to 10wt% Al, and the balance Fe (see, for example, Patent Document 1).

[0006] The FeSiAl alloy (Sendust) has the central composition (Fe 85 Al 5.38 S 9.62 The numbers are in wt %, and it is known that the magnetic permeability is 30,000 or more (for example, see Non-Patent Document 4). In addition, FeSiAl alloy (Sendust) has K1 and saturation magnetostriction constant λ s It is known that the soft magnetic properties are very sensitive to the composition and the heat treatment temperature during production (see, for example, Non-Patent Document 5). It is also known that the higher the heat treatment temperature during production, the higher the atomic order. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] https: / / doi.org / 10.1103 / PhysRevLett.93.111112 , Google Scholar Crossref , CAS 30. Kosuke Fujiwara, Mikihiko Oogane, Saeko Yokota, Takuo Nishikawa, Hiroshi Naganuma, and Yasuo Ando, ​​“ Fabrication of magnetic tunnel junctions with a bottom synthetic antiferro-coupled free layers for high sensitive magnetic field sensor devices ”, J. Appl. Phys., 2012, Vol. 111 , 07C7

Outdoor Tool2

Outdoor Tools3

Outdoor Tools 4

[0008] [Patent Document 1] Patent No. 120006 Summary of the Invention [Problem to be solved by the invention]

[0009] The alloys described in Non-Patent Documents 1 to 3 have been used as materials for the free layer of MTJ elements, but with the aim of further increasing the sensitivity of the magnetic sensor, it is hoped that alloys that have not been used for the free layer so far, but that have good soft magnetic properties comparable to conventional alloys and can be used for the free layer, will be found.

[0010] The present invention has been made in light of these problems, and aims to provide an FeSiAl alloy thin film that has good soft magnetic properties and can be used in a free layer of an MTJ element, a method for manufacturing an FeSiAl alloy thin film, and a magnetic sensor that includes an FeSiAl alloy thin film in the free layer of an MTJ element and a method for manufacturing the magnetic sensor. [Means for solving the problem]

[0011] The inventors have succeeded for the first time in producing a thin film of sendust having a thickness on the order of nanometers (100 nm or less), something that had not been possible until now. Upon examining the magnetic properties of this thin film of sendust, they found that by adjusting the composition it could have good soft magnetic properties, which led to the present invention.

[0012] That is, the FeSiAl alloy thin film according to the present invention is characterized by containing 7 wt% to 10 wt% Si, 4 wt% to 8 wt% Al, the remainder being Fe and unavoidable impurities, and having a film thickness of 20 nm to 100 nm.

[0013] The method for producing an FeSiAl alloy thin film according to the present invention is characterized in that a thin film containing 7 wt% to 10 wt% Si, 4 wt% to 8 wt% Al, with the remainder being Fe and unavoidable impurities, and having a thickness of 20 nm to 100 nm is formed on a substrate by sputtering, and then a heat treatment is performed at a temperature of 350°C to 500°C.

[0014] The FeSiAl alloy thin film according to the present invention can be suitably manufactured by the manufacturing method of the FeSiAl alloy thin film according to the present invention. The FeSiAl alloy thin film according to the present invention has an anisotropic magnetic field H that is equal to or smaller than that of the NiFe alloy described in Non-Patent Document 1 and the CoFeSiB alloy described in Non-Patent Document 3. k It has good soft magnetic properties. Therefore, by using it in the free layer of an MTJ element, a magnetic sensor with good sensitivity can be obtained. In addition, it can be manufactured more cheaply than NiFe alloy, CoFeB alloy, and CoFeSiB alloy.

[0015] The magnetic sensor according to the present invention is a magnetic sensor that utilizes a magnetic tunnel junction element having a fixed layer whose magnetization direction is fixed, a free layer whose magnetization direction is changeable, and an insulating layer disposed between the fixed layer and the free layer, and is characterized in that the free layer includes a FeSiAl alloy thin film.

[0016] The magnetic sensor according to the present invention has a new configuration in which the free layer contains a FeSiAl alloy thin film. In the magnetic sensor according to the present invention, the FeSiAl alloy thin film contained in the free layer is preferably the FeSiAl alloy thin film according to the present invention. In this case, the sensor has a particularly good sensitivity.

[0017] The manufacturing method of the magnetic sensor according to the present invention is a method for manufacturing the magnetic sensor according to the present invention, which is characterized in that the free layer, the insulating layer and the fixed layer are formed on a substrate by sputtering, in this order or in the reverse order, and then a heat treatment is performed at a temperature of 275°C or higher and 375°C or lower.

[0018] The method for manufacturing a magnetic sensor according to the present invention can obtain a magnetic sensor with a new configuration that has never been seen before, in which the free layer contains a thin FeSiAl alloy film. When forming the free layer, the method for manufacturing a magnetic sensor according to the present invention preferably includes sputtering to form a thin film having a thickness of 20 nm to 100 nm, containing 7 wt% to 10 wt% Si, 4 wt% to 8 wt% Al, and the remainder being Fe and unavoidable impurities, and then performing a heat treatment at a temperature of 350°C to 500°C. In this case, a free layer containing the thin FeSiAl alloy film according to the present invention can be formed. Therefore, a magnetic sensor with particularly good sensitivity can be obtained. Effect of the Invention

[0019] According to the present invention, it is possible to provide an FeSiAl alloy thin film having good soft magnetic properties and usable for a free layer of an MTJ element, a method for manufacturing an FeSiAl alloy thin film, and a magnetic sensor including an FeSiAl alloy thin film in the free layer of an MTJ element and a method for manufacturing the magnetic sensor. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a longitudinal sectional view showing a sample for investigating magnetic properties, etc., of an FeSiAl alloy thin film according to an embodiment of the present invention. [Diagram 2] 1A shows the XRD spectrum of sample 1, the XRD spectrum of sample 2, the XRD φ scan pattern of sample 1, and the XRD φ scan pattern of sample 2 at each heat treatment temperature Ta of the FeSiAl alloy thin film according to the embodiment of the present invention. [Diagram 3]1A is a graph showing the relationship between the average surface roughness (Ra) and the heat treatment temperature Ta of samples 1 and 2 of the FeSiAl alloy thin film according to the embodiment of the present invention, and FIG. 1B is an AFM image of sample 2 when the heat treatment temperature Ta is 400° C. [Figure 4] 1A and 1B show (a) an XRD spectrum and (b) an AFM image of the FeSiAl alloy thin film according to the embodiment of the present invention, when the heat treatment temperature Ta of sample 3 is 400° C. [Diagram 5] 1 shows magnetization curves (MH curves) of (a) Sample 1 and (b) Sample 2 of the FeSiAl alloy thin film according to the embodiment of the present invention at the heat treatment temperature Ta. [Figure 6] 1 shows a magnetization curve (MH curve) of sample 3 of the FeSiAl alloy thin film according to the embodiment of the present invention when the heat treatment temperature Ta is 400° C. [Figure 7] 1A is a graph showing the relationship between the anisotropy magnetic field Hk and the heat treatment temperature Ta of samples 2 and 5 of the FeSiAl alloy thin film according to the embodiment of the present invention, and FIG. 1B is a graph showing the relationship between the magnetocrystalline anisotropy constant K1 and the heat treatment temperature Ta of samples 2 and 5. [Figure 8] 1A to 1C are longitudinal cross-sectional views showing samples (a) to (c) of a magnetic tunnel junction (MTJ) element for determining a TMR ratio and a sensor sensitivity of a magnetic sensor according to an embodiment of the present invention. [Figure 9] 8(a) Magnetoresistance curves of the magnetic tunnel junction element shown in FIG. 8(a), (b) FIG. 8(b), and (c) FIG. 8(c) at each heat treatment temperature TMTJ. [Figure 10] 9 is a graph showing the relationship between the sensor sensitivity of the magnetic tunnel junction element shown in FIGS. 8(a) to 8(c) and the heat treatment temperature TMTJ. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiment of the present invention will be described based on examples. 1 to 10 show an FeSiAl alloy thin film and a magnetic sensor according to an embodiment of the present invention.

[0022] The FeSiAl alloy thin film according to the embodiment of the present invention contains 7 wt % to 10 wt % Si, 4 wt % to 8 wt % Al, the remainder being Fe and unavoidable impurities, and has a thickness of 20 nm to 100 nm.

[0023] The magnetic sensor according to the embodiment of the present invention is a magnetic sensor using a magnetic tunnel junction element having a fixed layer whose magnetization direction is fixed, a free layer whose magnetization direction is variable, and an insulating layer disposed between the fixed layer and the free layer, and the free layer includes a FeSiAl alloy thin film. The FeSiAl alloy thin film is preferably the FeSiAl alloy thin film according to the embodiment of the present invention. EXAMPLES

[0024] The FeSiAl alloy thin film according to the embodiment of the present invention was manufactured, and its magnetic properties, etc. were examined. As shown in Fig. 1, samples 1 to 5 were manufactured by laminating, in this order, an MgO layer 12 having a thickness of 20 nm, an FeSiAl alloy thin film 13 having a thickness of 30 nm, and a Ta layer 14 having a thickness of 5 nm on an MgO substrate 11 by magnetron sputtering. After the deposition, the FeSiAl alloy thin film 13 of each sample was heated at a temperature of 300 to 500°C (T a ) for one hour. The composition of the FeSiAl alloy thin film 13 of each sample is shown in Table 1. The composition of the FeSiAl alloy thin film 13 was determined by inductively coupled plasma (ICP) analysis.

[0025] [Table 1]

[0026] The FeSiAl alloy thin films 13 of Samples 1 to 3 were subjected to measurement by X-ray diffraction method and surface observation by AFM (atomic force microscope). aThe XRD spectra at 300°C, 400°C, and 500°C are shown in Fig. 2(a) and (b), respectively, and the XRD φ scan patterns are shown in Fig. 2(c) and (d), respectively. a The average surface roughness (R a ) in Fig. 3(a), and the heat treatment temperature T a FIG. 3(b) shows an AFM image of the FeSiAl alloy thin film 13 when the heat treatment temperature T a The XRD spectrum and AFM image of the FeSiAl alloy thin film 13 at 400° C. are shown in FIG. 4( a ) and ( b ), respectively.

[0027] As shown in Figures 2(a) and (b), the FeSiAl alloy thin film 13 of Samples 1 and 2 had a (004) peak indicating the A2 structure and a (002) peak indicating the B2 structure at any heat treatment temperature of 300 to 500°C. a The FeSiAl alloy thin film 13 at a heat treatment temperature of 400°C also had a (004) peak indicating the A2 structure and a (002) peak indicating the B2 structure. As shown in Figures 2(c) and (d) in the FeSiAl alloy thin films 13 of samples 1 and 2, peaks indicating the D03 ordered structure were observed at heat treatment temperatures of 400 to 500°C. From these results, it can be seen that the FeSiAl alloy thin film 13 has a (004) peak indicating the A2 structure and a (002) peak indicating the B2 structure at a heat treatment temperature of 400 to 500°C. a At 300°C, the A2 and B2 structures are mixed, and the heat treatment temperature T a When the temperature is between 400 and 500°C, it is believed that the A2, B2, and D03 structures are mixed.

[0028] In addition, as shown in Figs. 3(a), (b) and 4(b), the FeSiAl alloy thin films 13 of Samples 1 to 3 had an average surface roughness (R a ) was about 0.1 to 0.6 nm, and it was confirmed that the surface roughness was very small compared to the film thickness (30 nm).

[0029] Next, the magnetization curves (MH curves) of the FeSiAl alloy thin films 13 of Samples 1 to 3 were obtained. a The magnetization curves for the heat treatment temperatures T a 6 shows the magnetization curve of the FeSiAl alloy thin film 13 at 400° C. Each magnetization curve was measured along the

[0100] direction (in-plane direction).

[0030] As shown in FIG. 5, the FeSiAl alloy thin film 13 after the heat treatment of the samples 1 and 2 has a coercive force (H c ) is 6 Oe or less, and except for sample 1, which was heat-treated at 500°C, the coercivity (H c ) was confirmed to be 4 Oe or less. Also, as shown in FIG. 6, the sample 3 heat-treated at 400° C. had a coercive force (H c ) was confirmed to be about 1.6 Oe. These values ​​of coercivity are comparable to those of the NiFe alloy in Non-Patent Document 1 and the CoFeSiB alloy in Non-Patent Document 3, and it can be said that the FeSiAl alloy thin film 13 has good soft magnetic properties.

[0031] Next, the FeSiAl alloy thin film 13 of Samples 2 and 5 was subjected to the heat treatment at the heat treatment temperature T a The samples with temperatures between 300 and 500°C were measured at room temperature using a vibrating sample magnetometer (VSM). From the measurement results, the anisotropic magnetic field H k Furthermore, the anisotropy magnetic field H k From H k =2×K1 / M s (M s The magnetocrystalline anisotropy constant K1 was calculated using the formula: k and the magnetocrystalline anisotropy constant K1 and the heat treatment temperature T a The relationship between the anisotropic magnetic field H of the NiFe alloy of Non-Patent Document 1 and the CoFeSiB alloy of Non-Patent Document 3 is shown in Fig. 7(a) and (b), respectively. k The values ​​of are also shown.

[0032] As shown in FIG. 7(a), the FeSiAl alloy thin film 13 is heated at a temperature T a At temperatures between 350 and 500°C, the anisotropic magnetic field H is equal to or smaller than that of NiFe-based alloys and CoFeSiB-based alloys. k As shown in FIG. 7(b), the FeSiAl alloy thin film 13 was heated at a temperature T a It was confirmed that the magnetocrystalline anisotropy constant K1 was concentrated near zero and the magnitude of K1 was a very small value when the temperature was 350° C. to 500° C. From this result, it can be said that the FeSiAl alloy thin film 13 has good soft magnetic properties. EXAMPLES

[0033] 8(a) to (c), three magnetic tunnel junction (MTJ) elements were fabricated using the FeSiAl alloy thin film 13 of sample 3 shown in Table 1 as the free layer, and the TMR ratio and sensor sensitivity were determined. Each of the fabricated MTJ elements has the following structure from the bottom layer to the top layer. Fig. 8(a): MgO-sub. / MgO(20) / FeSiAl(30) / MgO(2.0) / Co 25 Fe 75 (5) / IrMn(10) / Ta(5) / Ru(10) Figure 8(b): SiO2-sub. / Ta(5) / CoFeB(5) / MgO(20) / FeSiAl(30) / CoFeB(1.0) / MgO(2.0) / CoFeB(3) / Ru(0.85) / CoFe(5) / IrMn(10) / Ta(5) / Ru(10) Figure 8(c): SiO2-sub. / Ta(5) / CoFeB(5) / MgO(20) / FeSiAl(30) / MgO(2.0) / CoFeB(3) / Ru(0.85) / CoFe(5) / IrMn(10) / Ta(5) / Ru(10) The numbers in parentheses indicate the film thickness in nm.

[0034] Each MTJ element has a planar area of ​​20×40 to 40×80 μm 2 After each layer was deposited by DC / RF magnetron sputtering, the layers were heat-treated at temperatures between 250°C and 425°C (T MTJ ) for fabrication. The layer between the substrate (sub.) 21 and the FeSiAl (30) layer of each MTJ element is the underlayer 22, which is provided to smooth the surface roughness of the substrate 21 and to enhance the crystal orientation of the FeSiAl (30) layer. The MgO (20) of the underlayer 22 in Figures 8(b) and (c) was formed and then heat-treated at a temperature T of 600 °C. MgO It is formed by heat treatment at .

[0035] The FeSiAl(30) layer in FIG. 8(a) and FIG. 8(c) and the FeSiAl(30) / CoFeB(1.0) layer in FIG. 8(b) on the underlayer 22 are the free layer 23, and the magnetization direction is changeable. The FeSiAl(30) layer of the free layer 23 is subjected to a heat treatment at a temperature T of 400° C. after deposition. a The MgO(2.0) layer on the free layer 23 is the insulating layer 24. The Co layer on the insulating layer 24 is 25 Fe 75 8(b) and (c) are the pinned layer 25, whose magnetization direction is fixed. The IrMn(10) on top of the pinned layer 25 is the antiferromagnetic layer 26. The Ta(5) / Ru(10) layer on top of the antiferromagnetic layer 26 is the cap layer 27.

[0036] Various heat treatment temperatures T MTJ For each of the MTJ elements shown in Figs. 8(a) to (c) fabricated in the above, the magnetoresistance curves were obtained by sweeping the in-plane magnetic field H from -1000 Oe to +1000 Oe using the DC four-terminal method. The results are shown in Figs. 9(a) to (c), respectively. As shown in Fig. 9(a), the MTJ element shown in Fig. 8(a) exhibited a magnetoresistance curve of 0.01 mm at a heat treatment temperature T MTJ It was confirmed that the TMR ratio was 55% or more when the heat treatment temperature T MTJhas a TMR ratio of 30% or more at 250 to 350°C, and the heat treatment temperature T MTJ It was confirmed that the maximum TMR ratio was 51.0% when the heat treatment temperature T was 300°C. In addition, as shown in the inset of Fig. 9(b), a small reversal magnetic field reflecting the soft magnetic properties was confirmed. As shown in Fig. 9(c), the MTJ element shown in Fig. 8(c) exhibited a small reversal magnetic field at a heat treatment temperature T MTJ It was confirmed that when the temperature was 300°C, the TMR ratio was 30% or more, and the maximum TMR ratio was 35.9%. In addition, as shown in the inset of Fig. 9(c), a small reversal magnetic field reflecting the soft magnetic properties was confirmed at 350°C or less. Comparing Fig. 9(b) and Fig. 9(c), it was confirmed that the TMR ratio was improved by inserting a CoFeB(1.0) layer into the free layer 23.

[0037] From the results shown in Fig. 9, various heat treatment temperatures T MTJ The sensor sensitivity of each of the MTJ elements shown in FIGS. 8(a) to (c) fabricated by the above method was measured and is shown in FIG. 10. Note that FIG. 10 also shows the sensor sensitivity of the MTJ element using the NiFe-based alloy of Non-Patent Document 1. As shown in FIG. 10, each MTJ element was MTJ It was confirmed that the sensor had high sensitivity when the temperature was 375°C or lower. In particular, it was confirmed that the MTJ element shown in Figure 8(a) had a sensor sensitivity equivalent to that of an MTJ element using a NiFe-based alloy. From this, it can be said that a magnetic sensor with good sensitivity can be obtained by using an FeSiAl alloy thin film for the free layer of an MTJ element. [Explanation of symbols]

[0038] 11 MgO substrate 12 MgO layer 13 FeSiAl alloy thin film 14 Ta layer 21 Substrate 22 Base layer 23 Free layer 24 Insulating layer 25 Fixed layer 26 Antiferromagnetic layer 27 Cap Layer

Claims

1. A magnetic sensor using a magnetic tunnel junction element having a fixed layer whose magnetization direction is fixed, a free layer whose magnetization direction is changeable, and an insulating layer disposed between the fixed layer and the free layer, The free layer includes an FeSiAl alloy thin film, the FeSiAl alloy thin film includes 7 wt % to 10 wt % of Si, 4 wt % to 8 wt % of Al, and the remainder is Fe and unavoidable impurities, has a film thickness of 20 nm to 100 nm, and includes an A2 structure and a B2 structure. A magnetic sensor characterized by:

2. A method for manufacturing the magnetic sensor according to claim 1, comprising the steps of: forming the free layer, the insulating layer, and the fixed layer on a substrate by sputtering in this order or in the reverse order, and then performing a heat treatment at a temperature of 275° C. or more and 375° C. or less; A method for manufacturing a magnetic sensor.

3. 3. The method for manufacturing a magnetic sensor according to claim 2, characterized in that when forming the free layer, a thin film containing 7 wt% to 10 wt% Si, 4 wt% to 8 wt% Al, with the remainder being Fe and unavoidable impurities, and having a thickness of 20 nm to 100 nm is formed by sputtering, and then a heat treatment is performed at a temperature of 350°C to 500°C.

Citation Information

Patent Citations

  • JP120006B

  • JP1937、1

  • Soft magnetic thin film and magnetic head

    JP1991161909A

  • Ferromagnetic tunnel junction element sensor and its manufacture

    JP1999134620A

  • Perpendicalar magnetic recording medium and magnetic recording and reproducing device using the same

    JP2002042318A