Fabric, its manufacturing method, and textile product

A fabric structure with a central fiber surrounded by ultrafine fibers in a sea-island composite yarn addresses the shortcomings of synthetic fibers by achieving a smooth, elastic, and dyeable texture similar to silk, with enhanced softness and impermeability.

JP7578433B2Active Publication Date: 2024-11-06TEJIN FIBERS LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020137922
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-18
Publication Date
2024-11-06
Estimated Expiration
2040-08-18

AI Technical Summary

Technical Problem

Existing synthetic fibers lack the smooth texture, elasticity, dyeability, and natural fullness similar to silk, despite various attempts to improve their properties.

Method used

A fabric structure comprising a central fiber surrounded by ultrafine fibers, utilizing a sea-island composite yarn with a sea component that is removed post-processing, creating a multifilament fabric with a core-sheath type composite yarn structure.

Benefits of technology

The fabric achieves excellent dyeability, smooth and slippery texture, elasticity, and cilia-like properties, mimicking natural fibers like silk, with improved softness and impermeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578433000001
    Figure 0007578433000001
  • Figure 0007578433000002
    Figure 0007578433000002
  • Figure 0007578433000003
    Figure 0007578433000003
Patent Text Reader

Abstract

To provide a fabric having cilia excellent in smooth and slippery feeling, and dyeability, and favorably excellent even in tension and stiffness, expanding feeling, soft feeling, and even in opacity like a natural fiber typified by silk, a method of producing the same, and a textile product.SOLUTION: A fabric includes a multifilament including one or more fiber group(s) including a center fiber positioned at a center part, and a plurality of ultrafine fibers surrounding the center fiber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fabric having a smooth, slippery feel with ciliated fibers and excellent dyeability, and also having excellent firmness, volume, softness, and transparency like natural fibers such as silk, a method for producing the fabric, and a textile product. [Background technology]

[0002] Synthetic fibers such as polyester are widely used not only for clothing but also for industrial purposes due to their excellent physical and chemical properties, and are of great industrial value. However, these synthetic fibers have the disadvantage that the texture and luster of the fibers are monotonous compared to natural fibers such as silk and cotton, due to the fact that the single fiber fineness of the fibers is uniform and large, and the cross-sectional shape is simple.

[0003] In order to overcome these drawbacks, various attempts have been made, such as modifying the cross-sectional shape of synthetic fibers, crimping, and using composite fibers, but it is difficult to say that the objectives have been fully achieved.

[0004] For example, Patent Document 1 proposes forming a composite fiber of an easily degradable polymer and polyester, and then imparting a dry touch, squeaky texture and unique luster to woven and knitted fabrics by post-processing. Patent Document 2 also proposes improving the texture by imparting spots in the length direction of the fiber. Patent Document 3 also proposes a fiber with a thick-thin structure and grooves on the fiber surface, and a manufacturing method thereof, in order to obtain a fiber for woven and knitted fabrics that exhibits a higher squeaky texture, with silk as the target. These prior documents have been inventive and ingenious in order to obtain a soft, fluffy feel unique to natural fibers, but they are not yet satisfactory. On the other hand, Patent Document 4 seeks a unique soft touch and fineness by utilizing the characteristics of nanofibers, which are thinner than ultrafine fibers (microfibers) on the micron order, to seek a texture like a new type of textile, but the characteristics of nanofibers are significant, and it is not yet satisfactory in terms of the natural fluffiness, feel, appearance, and firmness seen in natural materials, which are the original objectives. Patent Document 5 proposes that a mixed yarn of large fiber diameter and sea-island fiber is woven and knitted, and then subjected to a sea-removal process to maintain mechanical properties. In this case, the sea-island fiber parts and the thick fiber bundle parts are unevenly distributed, and it is still not satisfactory in terms of natural fluffiness. Patent Document 6 proposes a method in which a sea-island fiber is prepared in advance such that small and large fiber diameters (island diameters) are mixed in the cross section of the sea-island fiber, and the sea-island fiber is knitted and woven, and then the sea-island fiber is removed. However, this method uses fibers with large fiber diameters (microfibers or larger), and is still not satisfactory in terms of fineness. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 61-239010 [Patent Document 2] Japanese Patent Application Publication No. 58-70711 [Patent Document 3] Japanese Patent Publication No. 59-192709 [Patent Document 4] International Publication No. 2013 / 021809 Brochure [Patent Document 5] JP 2007-262610 A [Patent Document 6] Japanese Patent Application Publication No. 5-331711 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above background, and an object of the present invention is to provide a method for producing a smooth, ciliated To provide a fabric having a smooth texture and excellent dyeability, and preferably excellent in firmness, volume, softness and transparency like natural fibers such as silk, a method for producing the fabric, and a textile product. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors conducted extensive research to achieve the above object, and as a result, discovered that the desired fabric could be obtained by cleverly devising the structure of the multifilaments that constitute the fabric. Further extensive research led to the completion of the present invention.

[0008] Thus, according to the present invention, "a central fiber located at the center and the central fiber Satellite-like surround 50 to 100 bottles and a multifilament including at least one fiber group including an ultrafine fiber.

[0009] In this case, it is preferable that the single fiber diameter of the ultrafine fiber is 5000 nm or less. It is also preferable that the single fiber diameter of the central fiber is 10 times or more that of the ultrafine fiber. In addition, in the fiber group, the central fiber is one, and the ultrafine fiber is 50~100 bottlesIt is preferable that the multifilament contains 10 or more of the fiber groups. It is preferable that the multifilament is twisted. It is preferable that the multifilament is contained in a fabric as a sheath portion of a core-sheath type composite yarn. It is preferable that the core portion of the core-sheath type composite yarn is made of a composite fiber composed of two components. It is preferable that any one of the fibers constituting the fabric contains a recycled polymer. It is preferable that the dyeability is 30 or less in terms of L value.

[0010] The present invention also provides a method for producing a fabric, which comprises obtaining a fabric using composite fibers comprising a central island component fiber located at the center, a plurality of ultrafine fiber island components surrounding the central island component fiber, and a sea component, and then subjecting the fabric to a sea component removal treatment.

[0011] The present invention also provides a textile product made from the above-mentioned fabric, the textile product being selected from the group consisting of women's blouses, dresses, party dresses, men's suits, jackets, slacks, innerwear, sportswear, interior items, and daily necessities. Effect of the Invention

[0012] According to the present invention, there can be obtained a fabric having excellent dyeability, firmness and stiffness like natural fibers such as silk, a smooth and slippery texture, a fluffy feel, a soft feel, and excellent transparency, a method for producing the fabric, and a textile product. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a diagram illustrating an example of a fiber group according to the present invention. [Diagram 2] 1 is a photograph, shown in place of a drawing, of a cross section of a multifilament constituting the fabric obtained in Example 1. [Diagram 3] 2 is a photograph, shown in place of a drawing, of a cross section of a multifilament constituting the fabric obtained in Comparative Example 1. [Figure 4]1 is a photograph, shown in place of a drawing, of a cross section of a multifilament constituting the fabric obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings, in which: FIG. Here, the number of the central fiber is preferably 1. Also, the number of the ultrafine fibers surrounding the central fiber in a satellite shape is preferably 10 or more (more preferably 30 to 100). preferable.

[0015] In addition, the single fiber diameter (r s In order to obtain an excellent soft feel, the single fiber diameter (r c ) is preferably 10 times or more (more preferably 10 to 50 times) that of the ultrafine fibers in order to improve firmness and dyeability. In the central fiber and / or ultrafine fibers, the cross-sectional shape of the single fiber is not limited and may be any of round, hollow (e.g. round hollow, triangular hollow, square hollow, etc.), and irregular (e.g. triangular, square, flat, cross, etc.). When the cross-sectional shape of the single fiber is an irregular cross section other than a round cross section, the diameter of the circumscribed circle is taken as the single fiber diameter. The single fiber diameter can be measured by photographing the cross section of the fiber with a transmission electron microscope.

[0016] The type of polymer forming the ultrafine fibers and the central fiber is not particularly limited, but polyester-based polymers are preferred in terms of fiber strength and color fastness. For example, polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polylactic acid, stereocomplex polylactic acid, polyester copolymerized with a third component, and the like are preferred. Such polyesters may be polyesters that have been material recycled or chemically recycled, or polyethylene terephthalate or polytrimethylene terephthalate that uses monomer components obtained from biomass, i.e., plant-derived substances, as described in JP-A-2009-091694. Furthermore, polyesters obtained using catalysts containing specific phosphorus compounds and titanium compounds or catalysts made of light metals such as titanium-based catalysts, as described in JP-A-2004-270097 and JP-A-2004-211268, may also be used. The polymer may contain one or more of the following, if necessary, within the scope of the object of the present invention: a micropore-forming agent, a cationic dye-enabling agent, a coloration inhibitor, a heat stabilizer, a fluorescent brightening agent, a matting agent, a colorant, a moisture absorbent, and inorganic fine particles.

[0017] In the present invention, the multifilament contains one or more (preferably 10 to 100) of the above fiber groups. Such a multifilament can be produced, for example, by the following method. First, the above-mentioned polymer is prepared as the island component polymer (polymer forming the ultrafine fibers and the central fiber). In this case, the above-mentioned polymer may contain various additives such as inorganic substances such as titanium oxide, silica, barium oxide, etc., colorants such as carbon black, pigments, dyes, etc., flame retardants, fluorescent whitening agents, antioxidants, and ultraviolet absorbing agents.

[0018] Examples of the sea component polymer include polymers that can be melt-molded and can be dissolved and extracted after spinning, such as copolymerized polyethylene terephthalate, polyamide, polystyrene and its copolymers, polyethylene, and polyvinyl alcohol. In this case, the weight ratio of the two components forming the composite fiber is preferably within the range of 80:20 to 20:80.

[0019] Next, each component is discharged from a spinneret having discharge holes for discharging the central fiber island component (preferably 1 to 3, particularly preferably 1), the ultrafine fiber island components (preferably 10 or more, more preferably 30 to 100) arranged radially (satellite-like) around the central fiber island component, and the sea component.

[0020] The extruded islands-in-the-sea composite fiber is solidified by cooling air, and is melt-spun at a speed of preferably 400 to 6000 m / min, and then wound up. The obtained undrawn yarn is either subjected to a separate drawing process to produce a composite fiber having the desired strength, elongation, and thermal shrinkage properties, or is taken up on a roller at a constant speed without being wound up, and then subjected to a drawing process before being wound up. In addition, false twist crimping may be performed. In such islands-in-the-sea type composite fibers, the single fiber fineness, the number of filaments, and the total fineness are preferably within the ranges of 0.5 to 10.0 dtex, 5 to 75 filaments, and 30 to 170 dtex (preferably 30 to 100 dtex), respectively. In the present invention, the multifilament is obtained by subjecting the islands-in-sea type composite fiber to a sea-removal treatment.

[0021] The fabric of the present invention is a fabric made using such a multifilament. In this case, it is most preferable that the fabric is composed only of the multifilament, and it is preferable that the multifilament accounts for 30% by weight or more (more preferably 40% by weight or more) of the fabric weight.

[0022] The total cover factor CF of the fabric (woven or knitted fabric) is preferably 1000 or more (more preferably 1000 to 3000). The cover factor CF is calculated by the following formula. CF=(DWp / 1.1) 1 / 2 ×MWp+(DWf / 1.1) 1 / 2 ×MWf [DWp is the total warp thread size (dtex), MWp is the warp thread density (threads / 2.54cm), DWf is the total weft thread size (dtex), and MWf is the weft thread density (threads / 2.54cm).]

[0023] In this case, the islands-in-sea type composite fiber may be used as it is without twisting to weave a fabric, but if it is twisted at 500 to 3400 T / m, the sea component is dissolved to remove the sea, and the composite fiber takes on a spring shape, and the ultrafine fibers become cilia to cover the core fiber, improving the smooth and slippery feel, softness, lightness, and firmness, which is preferable. In this case, the twist coefficient is preferably within the range of 7000 to 30000. However, the twist coefficient is determined by the ratio of the number of twists (T / m) and (D / 1.1). 1 / 2 where D is the total fiber size (dtex) of the composite yarn.

[0024] The islands-in-the-sea composite fiber (multifilament) may be included in the fabric as the sheath of a core-sheath composite yarn, and the core of such a core-sheath composite yarn may be composed of a bicomponent composite fiber.

[0025] The weave structure of the fabric is not particularly limited, and examples of the weave structure of the fabric include three-pronged weaves such as plain weave, twill weave, and satin weave, altered weaves such as altered weave and altered twill weave, single-ply weaves such as warp double weave and weft double weave, warp pile weaves such as warp velvet, towel, and velour, and weft pile weaves such as velvet, weft velvet, velvet, and corduroy. Fabrics having these weave structures can be woven by a normal method using a normal loom such as a rapier loom or an air jet loom. The number of layers is not particularly limited, and may be a single layer or a multi-layer structure of two or more layers. The type of knitted fabric may be a weft knitted fabric or a weft knitted fabric. Preferred examples of weft knitting include plain knitting, rib knitting, double-sided knitting, purl knitting, tuck knitting, floating knitting, one-sided rib knitting, lace knitting, and brushed knitting, while preferred examples of warp knitting include single denbigh knitting, single atlas knitting, double cord knitting, half tricot knitting, fleece knitting, and jacquard knitting. Knitting can be performed by a conventional method using a conventional knitting machine such as a circular knitting machine, a flat knitting machine, a tricot knitting machine, or a raschel knitting machine. The number of layers is not particularly limited, and may be a single layer or a knitted fabric having a multi-layer structure of two or more layers.

[0026] When the fabric is a woven fabric, the density of the final woven fabric is preferably a warp density of 130 threads / 2.54 cm or more (preferably 130 to 200 threads / 2.54 cm) and a weft density of 90 threads / 2.54 cm or more (100 to 150 threads / 2.54 cm), as this improves the transparency-proofing.

[0027] Next, the fabric is dyed and processed, and then the sea-removal process is carried out by an alkali reduction process to remove the sea-removal material. By forming the islands-in-the-sea composite fiber into a multifilament containing one or more fiber groups including a central fiber located at the center and a plurality of ultrafine fibers surrounding the central fiber, a fabric having a soft feel and a lightweight feel, in which the cilia of the ultrafine fibers cover the central fiber, can be obtained. At the same time, the fabric has excellent transparency prevention properties and sufficient color fastness. In this case, the central fiber having a large fiber diameter is dyed in a deep color, so that excellent dyeability and color fastness can be obtained. In particular, when the multifilament containing one or more fiber groups including a central fiber located at the center and a plurality of ultrafine fibers surrounding the central fiber is twisted, the firmness, fullness, softness, and transparency prevention properties like those of natural fibers such as silk are further improved.

[0028] Here, the dyeability is preferably 30 or less (more preferably 10 to 25) in terms of L value. The dye fastness is evaluated by washing fastness and moisture-sensitive rubbing fastness according to JISL-0844 and JISL-0849. Both fastnesses are preferably grade 4 or higher. The transparency resistance is preferably 65% ​​or more (more preferably 70% or more, particularly preferably 72 to 98%).

[0029] Next, the textile product of the present invention is any textile product selected from the group consisting of women's blouses, one-piece dresses, party dresses, men's suits, jackets, slacks, innerwear, sportswear, interior items, and daily necessities, which uses the above-mentioned fabric. Since such textile products use the above-mentioned fabric, they have excellent dyeability, firmness like natural fibers, a dry texture with ciliary hairs, volume, softness, and opacity. EXAMPLES

[0030] Examples and Comparative Examples of the present invention will now be described in detail, but the present invention is not limited thereto. The measurement items in the examples were measured by the following methods.

[0031] <Staining L value> The L value of the test cloth was measured using a Macbeth color-Eye model M-2020 (manufactured by Kollmorgen, USA) with a light source of D65 and a 10-degree visual field. The n number was 5, and the average value was calculated.

[0032] <Color fastness> The color fastness to washing and humidity-sensitive rubbing fastness, discoloration and staining were measured according to JIS L-0844 and L-0849. Grade 4 or above was considered a pass.

[0033] <Transparency> The transparency was measured according to JIS L-1923. For multifilament woven fabrics with a total cover factor of 1200 or more, a value of 70% or more was judged to be excellent.

[0034] <Harikoshi (tight waist)> Sensory evaluation by five testers was conducted and the results were rated on a three-level scale: "excellent," "slightly inferior," and "poor." The most common rating was used as the conclusion.

[0035] [Example 1] The island component was polyethylene terephthalate (melt viscosity at 280°C: 1200 poise, matting agent content: 0 wt%) made from recycled materials derived from PET bottles, and the sea component was polyethylene terephthalate (melt viscosity at 280°C: 1750 poise) copolymerized with 6 mol% 5-sodium sulfoisophthalic acid and 6 wt% polyethylene glycol with a number average molecular weight of 4000. Two types of fiber diameters, island 1 and island 2 (fiber diameters of island 1 and island 2 are 10 times or more) were arranged in a satellite shape with one island 1 (for central fiber) surrounded by 50 island 2 (for ultrafine fiber) (dissolution rate ratio (sea / island) = 230), sea:island = 50:50, number of islands = 51. The sea-island type composite undrawn fiber (number of filaments: 27) was melt spun at a spinning temperature of 280°C and a spinning speed of 1500 m / min, and then wound up once. The obtained undrawn yarn was roller drawn at a drawing temperature of 80°C and a draw ratio of 2.5 times, then heat-set at 150°C and wound up. The obtained islands-in-sea type composite fiber (drawn yarn) had a total fineness of 73 dtex / 27 fil, and when the fiber cross section was observed with a transmission electron microscope (TEM), the islands were round, with the diameter of island 1 being 10,000 nm and the diameter of island 2 being 700 nm. In this case, the ratio of the single fiber diameters of the two islands was 14. Next, the composite fiber was given a twist of 3100 T / m (twist coefficient 25180) and twist-stopped at 90°C, then arranged as warp and weft yarns, and woven into a plain weave with a warp density of 105 / 2.54 cm and a weft density of 90 / 2.54 cm, then pre-relaxed at 60°C, flow-relaxed at 120°C, pre-set at 170°C, alkali-reduced (reduced by 43%), dyed at 130°C with a black disperse dye, and finally set at 170°C. The finished fabric had a warp density of 139 / 2.54 cm and a weft density of 101 / 2.54 cm. The fineness of the warp and weft yarns after processing was measured, and was about 40 dtex due to the dissolution and disappearance of the sea part by the weight reduction processing. Furthermore, when the woven structure was confirmed with an electron microscope, it was found that the multifilament consisted of 27 groups of fibers, each group including one central fiber located at the center and 50 ultrafine fibers surrounding the central fiber. Also, voids were confirmed between the individual fibers in the multifilament (Fig. 2, Photo 1). The dyeability was measured by the L value, which was 21.When the fastness to washing and humidity-sensitive rubbing was checked, the fastness to discoloration and staining was excellent, with both being grade 4 or higher. The total cover factor of this fabric was 1447, and the fabric's opacity was 75.8%, an excellent result. Furthermore, the evaluation result for firmness was "excellent," and the fabric had a smooth, slippery texture and excellent bulk.

[0036] [Example 2] The yarn was spun in the same manner as in Example 1, and the yarn was woven in a plain weave with a warp density of 120 / 2.54 cm and a weft density of 99 / 2.54 cm without twisting. The yarn was then pre-relaxed at 60°C, flow-relaxed at 120°C, pre-set at 170°C, and reduced in weight by alkali (weight reduction rate: 48%). The yarn was dyed at 130°C using a black disperse dye, and then finished by final setting at 170°C. The finished fabric had a warp density of 136 / 2.54 cm and a weft density of 108 / 2.54 cm. The fineness of the warp and weft yarns after processing was measured, and was found to be 38 dtex due to the dissolution and disappearance of the sea portion caused by the weight reduction process. The ratio of the single fiber diameters of the two islands was 14. The dyeability was L value 22, and when the physical properties of the fabric were checked, the fastnesses were graded 4 or higher for discoloration and staining, which was excellent, but the stiffness was rated as "slightly poor." The total cover factor of this fabric was 1471, and when checked, the transparency was found to be 70%, but based on the fabric cover factor of Example 1, it was 68.8%, which was a slightly inferior result.

[0037] [Comparative Example 1] Using polyethylene terephthalate (melt viscosity at 280°C: 1200 poise, matting agent content: 0 wt%) as the island component and polyethylene terephthalate (melt viscosity at 280°C: 1750 poise) copolymerized with 6 mol% 5-sodium sulfoisophthalic acid and 6 wt% polyethylene glycol having a number average molecular weight of 4000 as the sea component, (dissolution rate ratio (sea / island) = 230), sea:island = 30:70, number of islands = 8360, the island parts having the same fiber diameter were melt spun at a spinning temperature of 280°C and a spinning speed of 1500 m / min, and temporarily wound up. The obtained undrawn yarn was roller drawn at a drawing temperature of 80°C and a draw ratio of 2.5 times, then heat set at 150°C and wound up. The resulting islands-in-the-sea composite fiber multifilament (drawn yarn) had a total fineness of 56 dtex / 10fil, and when the fiber cross section was observed by a transmission electron microscope (TEM), the islands were found to be round and had a diameter of 700 nm. Next, the composite fiber yarn was twisted at 3100 T / m (twist coefficient 21920) and set at 90°C, and then arranged as warp and weft yarns and woven into a plain weave with a warp density of 130 / 2.54 cm and a weft density of 99 / 2.54 cm. The weft density was then pre-relaxed at 60°C and liquid spun at 120°C. The fabric was then subjected to flow relaxation, pre-setting at 170°C, alkali weight reduction (weight reduction rate 40%), dyed at 130°C using a black disperse dye, and then final set at 170°C. The finished fabric had a warp density of 195 / 2.54cm and a weft density of 110 / 2.54cm. The fineness of the warp and weft yarns after processing was measured and found to be 33dtex due to the dissolution and disappearance of the sea part due to the weight reduction processing. Furthermore, when the fabric structure obtained was confirmed with an electron microscope, it was confirmed that there were no gaps between the constituent multifilaments (Figure 3, Photo 2). The dyeability was poor with an L value of 35, and the color development was poor, and the various fastnesses were grade 2 for both discoloration and staining. The total cover factor of this fabric was 1671, and when the opacity was confirmed, it was 79%, but based on the fabric cover factor of Example 1, it was 68.4%, which was a slightly inferior result. The stiffness was "inferior," with a slimy texture typical of extremely fine fibers, and the fabric had a weak texture with no bulk.

[0038] [Comparative Example 2] Polyethylene terephthalate (melt viscosity at 280°C: 1200 poise, matting agent content: 1.8% by weight) with a round cross section was melt spun at a spinning temperature of 280°C and a spinning speed of 1500 m / min, and then wound up. The resulting undrawn yarn was roller-drawn at a drawing temperature of 80°C and a draw ratio of 2.5 times, and then heat-set at 150°C and wound up. The resulting round cross section multifilament (drawn yarn) had a total fineness of 44 dtex / 36fil. The stretched yarn was then given a twist of 3100 T / m (twist coefficient 19606) and twist-stopped at 90°C, after which the yarn was arranged as warp and weft yarns and woven into a plain weave with a warp density of 105 threads / 2.54 cm and a weft density of 90 threads / 2.54 cm. The yarn was then pre-relaxed at 60°C, flow-relaxed at 120°C, pre-set at 170°C, and reduced in weight by alkali (weight reduction rate 10%). The yarn was then dyed using a black disperse dye at 130°C, and finally set at 170°C for finishing. The finished fabric had a warp density of 167 threads / 2.54 cm and a weft density of 115 threads / 2.54 cm (Figure 4, Photo 3). When dyeability was measured using the L value, the L value was 16, and the various fastnesses for discoloration and staining were equivalent to those of Example 1. The total cover factor of this fabric was 1784, and when its transparency was confirmed it was 73%, but when the fabric cover factor of Example 1 was used as the standard, it was 59%, making it a more transparent fabric. The firmness was "excellent," but the texture was not soft and the fabric had no bulk.

[0039] [Comparative Example 3] Polyethylene terephthalate (melt viscosity at 280°C: 1200 poise, matting agent content: 1.8% by weight) with a round cross section was melt spun at a spinning temperature of 280°C and a spinning speed of 1500 m / min, and then wound up. The resulting undrawn yarn was roller-drawn at a drawing temperature of 80°C and a draw ratio of 2.5 times, and then heat-set at 150°C and wound up. The resulting round cross section multifilament (drawn yarn) had a total fineness of 33 dtex / 24 fil. Next, the drawn yarn was twisted to 3100 T / m (twist coefficient 16979) and twist-stopped at 90°C, then arranged as warp and weft yarns, and woven in a plain weave with a warp density of 130 / 2.54 cm and a weft density of 99 / 2.54 cm, then pre-relaxed at 60°C, flow-relaxed at 120°C, pre-set at 170°C, dyed at 130°C with a black disperse dye, and finally set at 170°C. The finished fabric had a warp density of 134 / 2.54 cm and a weft density of 197 / 2.54 cm. The dyeability was measured by the L value, which was 18, and the various fastnesses were grade 4. The total cover factor of this woven fabric was 1320, and the opacity was confirmed to be 63%, but based on the fabric cover factor of Example 1, it was 69.1%, which was a slightly inferior result. The fabric had "excellent" firmness, but no hairs at all, and had the characteristic synthetic feel of neither softness nor bulk.

[0040] [Comparative Example 4] Polyethylene terephthalate (melt viscosity at 280°C: 1200 poise, matting agent content: 1.8% by weight) was melt-spun at 280°C using a normal spinning device. The yarn was taken up at a speed of 1.6 m / min, wound up without stretching, and a semi-stretched polyester yarn of 56 dtex / 36 fil (cross-sectional shape of single fiber: round cross-section) was obtained. Next, the polyester yarn was used to carry out simultaneous stretch false twist crimp processing under the conditions of a stretch ratio of 1.6 times, a false twist number of 2500 T / m, a heater temperature of 180 ° C, and a yarn speed of 350 m / min. The obtained round cross-section multifilament (false twist yarn) had a total fineness of 33 dtex / 36 fil. Next, the false twist yarn was subjected to twisting at 300 T / m (twist coefficient 1643), which was arranged as a warp yarn and a weft yarn, and woven into a plain structure with a warp density of 135 / 2.54 cm and a weft density of 130 / 2.54 cm, and then preliminary relaxed at 60 ° C, liquid flow relaxed at 120 ° C, and preset at 170 ° C, dyed with a black disperse dye at 130 ° C, and then final set at 170 ° C to finish. The finished fabric had a warp density of 160 threads / 2.54 cm and a weft density of 140 threads / 2.54 cm. The total cover factor of this fabric was 1720. When the dyeability was measured by the L value, the L value was 17, and the various fastnesses were grade 4. However, the opacity prevention rate was high at 82% due to the false-twisted bulk, but when the fabric cover factor of Example 1 is used as the standard, it was 69%, which was slightly inferior to the fabric filling rate. The firmness of the fabric was "slightly inferior", and it had a bulky feel specific to false-twisted yarn and a dry touch. The fabric was completely free of cilia. [Industrial Applicability]

[0041] According to the present invention, there are provided a fabric having excellent dyeability, firmness and elasticity like natural fibers such as silk, a smooth and slippery texture, a fluffy feel, a soft feel, and excellent transparency, as well as a manufacturing method thereof and a textile product, and the industrial value of this fabric is extremely great.

Claims

1. A fabric comprising a multifilament including one or more fiber groups each including a central fiber located at the center and 50 to 100 ultrafine fibers surrounding the central fiber in a satellite shape.

2. The fabric according to claim 1 , wherein the ultrafine fibers have a single fiber diameter of 5000 nm or less.

3. 3. The fabric according to claim 1, wherein the central fiber has a single fiber diameter that is 10 times or more larger than that of the ultrafine fibers.

4. The fabric according to any one of claims 1 to 3, wherein the fiber group includes one central fiber and 50 to 100 ultrafine fibers.

5. The fabric according to any one of claims 1 to 4, wherein the multifilament contains 10 or more of the fiber groups.

6. The fabric according to any one of claims 1 to 5, wherein the multifilament is twisted.

7. The fabric according to any one of claims 1 to 6, wherein the multifilament is included in the fabric as a sheath portion of a core-sheath type composite yarn.

8. The fabric according to claim 7 , wherein in the core-sheath type composite yarn, the core portion is made of a composite fiber composed of two components.

9. The fabric according to any one of claims 1 to 8, wherein any fiber constituting the fabric contains a recycled polymer.

10. The fabric according to any one of claims 1 to 9, having a dyeability of 30 or less in terms of L value.

11. The method for producing a fabric according to any one of claims 1 to 10, further comprising the steps of: obtaining a fabric using composite fibers comprising a central island component fiber located at the center, a plurality of ultrafine fiber island components arranged so as to surround the central island component fiber, and a sea component; and then subjecting the fabric to a sea component removal treatment.

12. A textile product selected from the group consisting of women's blouses, dresses, party dresses, men's suits, jackets, slacks, innerwear, sportswear, interior goods, and daily necessities, which is made using the fabric according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Preparation of thick and thin yarn

    JP1983070711A

  • Fiber having surface groove and uneven thickness, and manufacture thereof

    JP1984192709A

  • Two-component composite fiber

    JP1986239010A

  • Polyester ternary conjugate fiber

    JP1989014321A

  • Conjugate fiber of different denier

    JP1993331711A