Fluorophosphate optical glasses, as well as optical preforms, elements, and devices

The optimized fluorophosphate optical glass composition addresses the issues of high density and instability in existing glasses by achieving low thermal expansion, high chemical stability, and resistance to crystallization, suitable for high-precision optical instruments.

JP7581189B2Active Publication Date: 2024-11-12CDGM OPTICAL GLASS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021517199
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-09-28
Publication Date
2024-11-12
Estimated Expiration
2038-09-28

AI Technical Summary

Technical Problem

Existing fluorophosphate optical glasses have high density, low chemical stability, high thermal expansion coefficient, and susceptibility to crystallization, making them unsuitable for high precision optical instruments.

Method used

A fluorophosphate optical glass composition with specific cation and anion ratios, including P5+, Al3+, Ba2+, Sr2+, Ca2+, Mg2+, and F-, O2-, and optional rare earth elements, optimized to achieve a refractive index of 1.42 to 1.45, Abbe number of 93 to 96, thermal expansion coefficient of 160×10-7/K or less, and density of 3.55 g/cm3 or less, with improved chemical stability and resistance to crystallization.

Benefits of technology

The optimized glass composition provides excellent chemical stability, low thermal expansion, high bubble degree, and resistance to crystallization, enabling high-quality optical elements and devices with reduced weight and volume.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581189000001
    Figure 0007581189000001
  • Figure 0007581189000002
    Figure 0007581189000002
  • Figure 0007581189000003
    Figure 0007581189000003
Patent Text Reader

Abstract

The present invention provides fluorophosphate glasses, optical preforms, elements, and devices in the field of optical glass. The optical glass comprises the following components in terms of cation molar percentage: 2 to 20% P 5+ and 20-40% Al 3+ and 0.5-10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ and containing the following components in mole percentage of anions: 83-95% F - and 5–17% O 2- The fluorophosphate optical glass has a refractive index (nd) of 1.42 to 1.45, an Abbe number (vd) of 93 to 96, and a viscosity of 3.55 g / cm 3 Density (ρ) below, foaming degree of grade B or higher, 160×10 -7 / K or less thermal expansion coefficient, water resistance of grade 2 or more (D W ) and has excellent crystallization resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of optical glasses, in particular to the technical field of fluorophosphate optical glasses, optical preforms, elements and devices. [Background technology]

[0002] Fluorophosphate optical glass is a new glass material with low refractive index and low dispersion. The glass can eliminate the special dispersion of secondary spectrum from the optical system, increase the resolution and improve the image quality of the optical system. It also has low softening properties and can be directly made into an aspheric lens by precision molding. It can also eliminate chromatic aberration, spherical aberration, and aberration, and reduce the volume and weight of the system.

[0003] Up to now, fluorophosphate optical glass has been widely applied in optical instruments with high-precision and high-resolution lenses, such as digital cameras, HD monitors, and astronomical telescopes, and has become a new photoelectric material with potential market prospects. Its specific applications in these fields have higher requirements for fluorophosphate optical glass. Existing public documents have reported fluorophosphate optical glasses with Abbe numbers of 80 or more. However, these fluorophosphate optical glasses have high density, low chemical stability and crystallization resistance, high thermal expansion coefficient, and low degree of bubbles, which easily cause damage during mold pressing and heating. Summary of the Invention

[0004] The object of the present invention is to provide a fluorophosphate optical glass, an optical preform, an element, and an instrument having a refractive index (nd) of 1.42 to 1.45 and an Abbe number (vd) of 93 to 96. The fluorophosphate optical glass provided by the present invention has low density, a low thermal expansion coefficient, a high degree of bubbles, excellent chemical stability and crystallization resistance, and is less susceptible to damage during die pressing and heat treatment, and can be mass-produced in a stable mode.

[0005] The present invention is implemented by the following technical solutions: For fluorophosphate optical glass, the cations are P 5+ , Al 3+ and alkaline earth metal ions, and the anion is F - and O 2- It contains the same thermal expansion coefficient (α 20°C~120℃ ) is 160 x 10 -7 / K or less, and the density (ρ) is 3.55 g / cm 3 Water resistance (D W ) is grade 2 or higher.

[0006] Fluorophosphate optical glasses are made up of the following molar percentages of cations: 2-20% P 5+ and 20-40% Al 3+ and 0.5-10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ and contains the following components in terms of anion molar percentage: 83-95% F - and 5–17% O 2- Contains: Ba 2+ / Ca 2+ is 0.11 to 0.155.

[0007] Fluorophosphate optical glasses are made up of the following molar percentages of cations: 2-20% P 5+ and 20-40% Al 3+ and 0.5-10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ and contains the following components in terms of anion molar percentage: 83-95% F - and 5–17% O 2- Contains: Ba 2+ / Ca 2+ is 0.11 to 0.155.

[0008] The fluorophosphate optical glass contains 0 to 6% Ln 3+ and 0-10% Na + and 0-10% Li + and 0-10% K + It contains Ln 3+ La 3+ , Gd 3+ , Y 3+ , and Yb 3+ One or more of the following:

[0009] Fluorophosphate optical glasses are made up of the following molar percentages of cations: 2-20% P 5+ and 20-40% Al 3+ and 0.5-10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ It contains 0-10% Na + and 0-10% Li + and 0-10% K + and 0-6%Ln 3+ It contains Ln 3+ La 3+ , Gd 3+ , Y 3+ , and Yb 3+ The glass is one or more of the following components in terms of molar percentage of anions: 83 to 95% F - and 5–17% O 2- Contains: Ba 2+ / Ca 2+ is 0.11 to 0.155.

[0010] Furthermore, the refractive index (nd) of the glass is from 1.42 to 1.45, preferably from 1.43 to 1.44, and the Abbe number (vd) is from 93 to 96, preferably from 94 to 95.5.

[0011] Furthermore, P 5+ 3-15% and / or Al 3+ 25-38% and / or Ba 2+1-8% and / or Sr 2+ 10-22% and / or Ca 2+ 20-33% and / or Mg 2+ is 2-12%, and / or Ln 3+ 0-5% and / or Na + 0-4% and / or Li + is 0.5 to 5%, and / or K + is 0-5%.

[0012] In addition, Ba 2+ / Ca 2+ but 0.12~0.15 , and / or Ba 2+ / (Ca 2+ +Mg 2+ ) is 0.08 to 0.13, and / or O 2- / F - is 0.105~0.2.

[0013] Furthermore, P 5+ 5-10% and / or Al 3+ 30-35% and / or Ba 2+ 1-5% and / or Sr 2+ 15-20% and / or Ca 2+ 25-30% and / or Mg 2+ is 5-10%, and / or Ln 3+ 0.5-3% and / or Na + 0.5-2% and / or Li + 0.5-3% and / or K + is 0 to 2%.

[0014] moreover, O 2- / F - but It is 0.11 to 0.18.

[0015] moreover, O 2- / F - but It is 0.11 to 0.15.

[0016] Furthermore, Y3+ is 0 to 5%, preferably 0 to 4%, and more preferably 0.5 to 3%, and La 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%, and Gd 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%, and Yb 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%.

[0017] In addition, F - The content is 85 to 92%, more preferably 87 to 91%, and O 2- The content is preferably 8 to 15%, more preferably 9 to 13%.

[0018] In addition, the thermal expansion coefficient (α 20℃~120℃ ) is 155 x 10 -7 / K or less, and the density (ρ) is 3.53 g / cm 3 The foam level is grade B or higher, preferably grade A or higher, and more preferably grade A0 or higher. The water resistance (D W ) is grade 1 or higher.

[0019] An optical preform is made from said fluorophosphate optical glass.

[0020] An optical element is fabricated from the fluorophosphate optical glass and the optical preform.

[0021] An optical instrument is made from the optical element.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] Through rational component design, the fluorophosphate optical glass provided by the present invention has excellent chemical stability, crystallization resistance, thermal expansion coefficient, and bubble degree. The fluorophosphate optical glass provided by the present invention has a refractive index (nd) of 1.42 to 1.45, an Abbe number (vd) of 93 to 96, a thermal expansion coefficient (α 20°C~120°C ) is 160 x 10 -7 / K or less, density (ρ) is 3.55g / cm 3 The following are cases where the degree of foam is grade B or higher and the water resistance (D W ) is grade 2 or higher. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] In order to clearly understand the objectives, technical solutions and advantages of the present invention, the present invention will be further described in conjunction with the following embodiments. It should be understood that the specific implementations described herein do not limit the present invention in any way, but are merely used to describe the present invention.

[0025] The following paragraphs explain the function and range limitations of all components contained in the fluorophosphate optical glasses provided by the present invention in conjunction with specific principles.

[0026] It should be noted that, in this specification, the content of each cation and the total content of the cations is expressed as the "molar percentage of cations," and the content of each anion and the total content of the anions is expressed as the "molar percentage of anions." The "molar percentage of cations" refers to the proportion of a particular cation among all cations, and the "molar percentage of anions" refers to the proportion of a particular anion among all anions.

[0027] It should be noted that the ionic valence of each component is not different from the other ionic valences, but is merely a typical value for convenience. The ionic valences of all components present in optical glasses have other possibilities in addition to the typical value. For example, P is present in the glass in the form of an ionic valence of 5, and therefore is typically referred to herein as "P 5+ ", but may have other ionic valence states and are also within the scope of protection of the present invention.

[0028] P 5+ plays a role as a network structure in the fluorophosphate glass, and O 2-Together with P, they constitute the main element of the glass frame and are important components capable of improving the mechanical properties of the glass while maintaining the forming stability of the glass. 5+ If the content is less than 2%, the crystallization tendency of the glass increases and the stability deteriorates. 5+ If the content is more than 20%, the properties of the glass are significantly affected, making it difficult to obtain the optical constants required by the present invention. Therefore, when considering the stability and optical properties of the glass, P 5+ The content is defined as 2 to 20%, preferably 3 to 15%, and more preferably 5 to 10%.

[0029] Al 3+ Al is an important component for improving the devitrification resistance and chemical stability in fluorophosphate glass. If its content is less than 20%, the chemical stability of the glass is reduced, and the lower limit is 20%, preferably 25%, and more preferably 30%. If its content is more than 40%, the required refractive index and Abbe number cannot be obtained due to the reduction in the contents of other components, and the conversion temperature Tg of the glass increases significantly, causing an increase in the molding temperature and an increase in opacity, brittleness, and wear hardness. 3+ The upper limit is 40%, preferably 38%, more preferably 37%, even more preferably 36%, and still more preferably 35%.

[0030] Ba 2+ , Sr 2+ , Ca 2+ , and Mg 2+ The main effects of alkaline earth metal ions such as , , etc. are to improve the chemical stability and crystallization resistance of the glass, enable the glass to reach the expected optical properties, control the refractive index and Abbe number, and optimize the manufacturing process of optical glasses.

[0031] Specifically, Ba 2+is beneficial to the devitrification resistance and the refractive index of the glass. If its content is lower than 0.5%, the chemical stability and devitrification resistance of the glass deteriorate. If its content is higher than 10%, the required refractive index and Abbe number cannot be achieved, while the specific gravity of the glass increases. Therefore, Ba 2+ The content is defined as 0.5 to 10%, preferably 1 to 8%, and more preferably 1 to 5%.

[0032] Sr 2+ is effective in improving the devitrification resistance of glass, and can effectively adjust the refractive index and specific gravity of glass. If its content is excessive, the refractive index and dispersion of glass will increase, making it difficult to achieve the expected chemical properties and reducing the chemical stability of glass. Therefore, in order to obtain better optical properties, Sr 2+ The content is defined as 5 to 25%, preferably 10 to 22%, and more preferably 15 to 20%.

[0033] Ca 2+ Ca can reduce the Abbe number and specific gravity of the glass, stabilize the glass formation, and improve the acid resistance and wear resistance of the glass. If its content is too low, the required optical properties cannot be achieved. If its content is too high, the devitrification resistance and chemical stability of the glass will be deteriorated. Therefore, Ca 2+ The content is defined as 15 to 35%, preferably 20 to 33%, and more preferably 25 to 30%.

[0034] Mg 2+ has the effect of improving the thermal stability and wear resistance of glass, and effectively improves glass formation, devitrification resistance, and glass processability. If its content is too low, the possibility of adjusting the processability is low, and the difficulty of glass processing increases. If its content is too high, the content of other alkaline earth metals is reduced, and the required optical properties cannot be achieved. Therefore, Mg 2+ The content is defined as 1 to 15%, preferably 2 to 12%, and more preferably 5 to 10%.

[0035] Regarding the types of alkaline earth metals added and the contents of various components, the inventors have found that four alkaline earth metals (Ba 2 , Sr 2+ , Ca 2+ , and Mg 2+ It has been found that the refractive index and Abbe number of the fluorophosphate optical glass provided by the present invention can be obtained by adding fluorine phosphate fluoride ...

[0036] In addition, according to the research findings, the inventors 2+ / Ca 2+ and Ba 2 / (Ca 2+ +Mg 2+ It was found that the ratio of Ba to Ba has a significant effect on the density, foaming degree, chemical stability, and crystallization resistance. 2+ / Ca 2+ If the ratio is higher than 0.155, the specific gravity of the glass increases, making it difficult to achieve the goal of weight reduction. 2+ / Ca 2+ If the ratio is less than 0.01, the glass is prone to bubble formation and the crystallization resistance is reduced. 2+ and Ca 2+ In order to balance the amount of Ba added, reduce the glass density, and improve the degree of bubbles and crystallization resistance, 2+ / Ca 2 is 0.01 to 0.155, preferably 0.03 to 0.155, further preferably 0.05 to 0.155, and even more preferably 0.1 to 0.15.

[0037] Ba 2 / (Ca 2+ +Mg 2+ ) ratio is higher than 0.13, Ba 2+ , Ca 2+ , and Mg 2+ The amount of Ba added is unbalanced, thus increasing the specific gravity of the glass. 2+ / (Ca2+ +Mg 2+ If the ratio of Ba is less than 0.08, the chemical stability of the glass deteriorates and the crystallization resistance decreases. Therefore, in order to reduce the density of the glass and improve the chemical stability and crystallization resistance, Ba is preferably used. 2 / (Ca 2+ +Mg 2+ ) is defined to be 0.08 to 0.13, preferably 0.09 to 0.125, and more preferably 0.1 to 0.12.

[0038] Li + , Na + , and K + Alkali metals such as Na, NaH, NaN, NaH ... + The content is defined as 0 to 10%, preferably 0 to 4%, and more preferably 0.5 to 2%. + The content is defined as 0 to 10%, preferably 0.5 to 5%, and more preferably 0.5 to 3%. + The content is 0 to 10%, preferably 0 to 5%, more preferably 0 to 2%, and even more preferably none is incorporated.

[0039] Ln as rare earth element 3+ (La 3+ , Gd 3+ , Yb 3+ , and Y 3+ ) are components that maintain low dispersion and improve the refractive index of glass. If their content is too high, the effect cannot be achieved. However, if they are added excessively, the refractive index of glass exceeds the required range. In addition, as the melting temperature increases, the chemical stability of glass decreases. Therefore, the rare earth elements Ln 3+ The total content of Y is defined as 0 to 6%, preferably 0 to 5%, and more preferably 0.5 to 3%. 3+ is 0 to 5%, preferably 0 to 4%, and more preferably 0.5 to 3%. 3+is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%.

[0040] In the range not impairing the glass properties of the present invention, 0 to 5% of Si other than the above is used. 4+ , B 3+ , Ti 4+ , Nb 5+ , W 6+ , Zr 4+ , Zn 2+ , Ge 4+ , Te 4+ , Ce 4+ , Sb 3+ , and Sn 4+ Other cations including may be added as necessary. However, transition metal components such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo, whether contained alone or in the form of a compound, will color the glass and absorb certain wavelengths in the visible light region, thereby reducing the characteristic of the present invention of improving visible light transmittance. Therefore, it is preferable that they are not actually contained in optical glasses that require wavelength transmittance in the visible region in particular.

[0041] The cations Pb, Th, Cd, Tl, Os, Be and Se have been used in recent years as hazardous chemicals in a controlled manner, which is necessary not only in the glass manufacturing process, but also in the processing procedures and post-manufacturing disposal for environmental protection measures. Therefore, when the impact on the environment is important, it is preferable that they are not actually included except for unavoidable incorporation. As a result, the optical glass does not actually contain substances that pollute the environment. Therefore, the optical glass provided by the present invention can be manufactured, processed and disposed of even if no standards are adopted as special environmental measures.

[0042] Next, the anion component will be described in detail.

[0043] In the fluorophosphate optical glass provided by the present invention, O 2- and F - is an anionic component, which is added to achieve the desired optical properties and glass stability.

[0044] Specifically, F - F is an important component that makes glass low dispersion and anomalous dispersion, and is effective in lowering the refractive index, temperature coefficient, and Tg. If its content is too low, it is difficult to reach the required properties. If its content is too high, the chemical stability of the glass will be weakened, and the thermal expansion coefficient and wear hardness will increase, especially in the melting process. The volatilization of F not only pollutes the environment, but also makes the internal composition of the glass non-uniform, causing abnormal data, streaks, and other defects. Therefore, F - The content is 83 to 95%, preferably 85 to 92%, and more preferably 87 to 91%.

[0045] O 2- is a necessary component for forming the network structure of the fluorophosphate optical glass. If its content is too low, the glass stability becomes insufficient, making it difficult to achieve the refractive index required in the present invention. If its content is too high, it becomes difficult to obtain the required dispersion and anomalous dispersion. Therefore, O 2- The content is defined as 5 to 17%, preferably 8 to 15%, and more preferably 9 to 13%.

[0046] Through research findings, the inventors 2- Against F - (O 2- / F - We found that the molar content of ) significantly affects the thermal expansion coefficient, moldability properties, and glass forming properties of fluorophosphate optical glasses. 2- / F - If the ratio is lower than 0.105, the thermal expansion coefficient becomes high and the moldability characteristics become insufficient. 2- / F -When the ratio is higher than 0.2, the glass forming properties are disadvantageous. Therefore, in order to reduce the thermal expansion coefficient of the glass, to avoid easy damage during mold pressing and heat treatment, and to improve the glass forming properties, O 2- / F - The ratio is defined as 0.105 to 0.2, preferably 0.11 to 0.18, and more preferably 0.11 to 0.15.

[0047] The anion is Cl - May contain Cl - is introduced in the form of chloride cations, preferably in the form of BaCl2, and may be employed in the present invention as a fining agent having a content of 0-1%.

[0048] The properties of the fluorophosphate optical glass provided by the present invention will now be described.

[0049] The refractive index (nd) and Abbe number (vd) are analyzed according to the test method specified in GB / T7962.1-2010.

[0050] Thermal expansion coefficient (α 20°C~120°C ) is analyzed according to the test methods specified in GB / T7962.16-2010.

[0051] The density (ρ) is analyzed according to the test method specified in GB / T7962.20-2010.

[0052] The degree of foaming is analyzed according to the test method specified in GB / T7962.8-2010.

[0053] Water resistance (D W ) is analyzed according to the test methods specified in GB / T17129.

[0054] The method for analyzing the crystallization resistance performance of glass provided by the present invention includes the following steps: Cut the sample glass to the specification of 20 x 20 x 10 mm, place it in a muffle furnace at a temperature of Tg + 230 ° C. and keep it warm for 30 minutes, take it out and put it in warm cotton for annealing. Then, visually observe the surface crystallization after cooling. Here, if there is no obvious crystallization, it is marked with "A", and if there is obvious crystallization, it is marked with "B".

[0055] After analysis, the fluorophosphate optical glass provided by the present invention has the following properties:

[0056] The refractive index (nd) of the glass is 1.42 to 1.45, preferably 1.43 to 1.44. The Abbe number (vd) is 93 to 96, preferably 94 to 95.5. The density (ρ) is 3.55 g / cm 3 Less than or equal to 3.53 g / cm 3 The degree of bubbles is at least grade B, preferably at least grade A, and more preferably at least grade A0. The thermal expansion coefficient (α 20°C~120°C ) is 160 x 10 -7 / K or less, preferably 155×10 -7 / K or less.

[0057] The melting and molding method of optical glass production is carried out by using techniques well known to those skilled in the art. This method involves weighing and uniformly mixing glass raw materials (carbonates, nitrates metaphosphates, fluorides, oxides, etc.) in the proportion of the total ions of the glass. Then, it is put into a smelting device (such as a platinum crucible) and cooled to less than 900°C after appropriate mixing, clarification, and homogenization at 900-1,250°C, and poured or poured into a mold. And finally, it is subjected to post-treatment including annealing, processing, etc., or directly pressed and molded through precision press molding technology.

[0058] The fluorophosphate optical glass provided by the present invention may be employed as a glass preform material for pressure molding, or the molten glass may be directly pressure molded. When the glass is used as a glass preform, there is no special restriction on the manufacturing and thermoforming methods, so that the known manufacturing and molding methods can be used.

[0059] The present invention also provides optical elements made from the optical glass according to methods well known to those skilled in the art, for example, melted and softened optical glass is directly subjected to pressure processing to produce optical elements, or glass preform materials made from the optical glass provided by the present invention are pressure processed to produce optical elements.

[0060] The present invention further provides optical instruments made from the manufactured optical elements, for example, various lenses such as biconvex lenses, biconcave lenses, plano-convex lenses, plano-concave lenses, and convex-concave lenses, as well as reflectors, prisms, and diffraction gratings, which may be applied in digital cameras, digital video cameras, camera phones, and other devices.

[0061] The following paragraphs describe the compositions and properties of the fluorophosphate optical glasses provided by the present invention in combination with specific implementations, but the present invention is not limited to the following embodiments.

[0062] [Embodiments of optical glass]

[0063] The compositions of the fluorophosphate optical glasses in the embodiments 1 to 37 of the present invention and the comparative examples 1 to 3, as well as the refractive index (nd), Abbe number (vd), density (ρ), degree of bubbles, thermal expansion coefficient, water resistance (D W ) and crystallization resistance are shown in Tables 1 to 4. The contents of all components are expressed in mol %. [Table 1] [Table 2] [Table 3] [Table 4]

[0064] [Embodiment of Optical Preform] The optical glass obtained in the embodiments 1 to 37 is cut to a predetermined size, and a release agent is uniformly applied to the surface.Then, the mold is heated and softened to be press-molded to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.Alternatively, the optical glass obtained in the embodiments 1 to 37 is formed into a pre-molded product for precision press molding, and then is precisely press-molded into lens and prism shapes through precision press molding and processing to produce preforms.

[0065] [Embodiments of Optical Elements] These resulting preforms in the optical preform embodiments are annealed to reduce distortion in the glass and fine-tune the optical properties, such as the refractive index, to the desired values.

[0066] Each preform is then ground and polished to form a variety of lenses and prisms, such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surfaces of the resulting optical elements may be coated with an anti-reflective coating.

[0067] [Embodiment of Optical Instrument] The optical components or optical members are formed by optical elements obtained in the embodiment of the optical element through optical design or through one or more optical elements. The optical components or optical members can be used in imaging devices, sensors, microscopes, medical technology, digital projection, communication, optical communication technology / information transmission, optics / illumination in the automotive field, photolithography, excimer lasers, wafers, computer chips and integrated circuits, and electronic devices containing such circuits and chips.

[0068] All the above are merely preferred embodiments of the present invention, and do not limit the scope of the present invention. All modifications, equivalent replacements, and improvements that do not depart from the spirit and principle of the present invention are within the protection scope of the present invention.

Claims

1. The cation is P 5+ And, Al 3+ and an alkaline earth metal ion, the anion being F - And, O 2- and the thermal expansion coefficient of optical glass (α 20℃~120℃ ) is 160 x 10 -7 / K or less, and the density (ρ) is 3.55 g / cm 3 Water resistance (D W ) is grade 2 or higher, The molar percentage of cations is as follows: 2-20% P 5+ and 20-40% Al 3+ and 0.5 to 10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ 0-5.75% Y 3+ , 0-5.11% La 3+ , 0-4.56% Gd 3+ , 0-4.23% Yb 3+ , 0-9.22% Na + , 0-8.89% Li + , 0-1.69% K + , and a total of 0-5% other cations, with the following molar percentages of anions: 83-95% F - and 5-17% O 2- and Ba 2+ / Ca 2+ is 0.11 to 0.155, and Ba 2+ / (Ca 2+ + Mg 2+ ) is 0.09 to 0.

125.

2. The molar percentage of cations is as follows: 2-20% P 5+ and 20-40% Al 3+ and 0.5 to 10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+0-5.75% Y 3+ , 0-5.11% La 3+ , 0-4.56% Gd 3+ , 0-4.23% Yb 3+ , 0-9.22% Na + , 0-8.89% Li + , 0-1.69% K + , and a total of 0-5% other cations, with the following molar percentages of anions: 83-95% F - and 5-17% O 2- and Ba 2+ / Ca 2+ is 0.11 to 0.155, and Ba 2+ / (Ca 2+ + Mg 2+ ) is 0.09 to 0.

125.

3. The molar percentage of cations is as follows: 2-20% P 5+ and 20-40% Al 3+ and 0.5 to 10% Ba 2+ and 5-25% Sr 2+ and 15-35% Ca 2+ and 1-15% Mg 2+ and 0-10% Na + and 0-10% Li + And 0 to 10% K + and 0 to 6% Ln 3+ and a total of 0-5% other cations, Ln 3+ La 3+ , Gd 3+ , Y 3+ , and Yb 3+ and one or more of the following components in terms of molar percentage of anion: 83-95% F - and 5-17% O 2- and Ba 2+ / Ca 2+ is 0.11 to 0.155, and Ba 2+ / (Ca 2+ + Mg 2+ ) is 0.09 to 0.

125.

4. 4. The optical fluorophosphate glass according to claim 1, characterized in that it has a refractive index (nd) of 1.42 to 1.45, preferably 1.43 to 1.44, and an Abbe number (vd) of 93 to 96, preferably 94 to 95.

5.

5. P 5+ and / or Al 3+ and / or Ba 2+ and / or Sr 2+ 10 to 22%, and / or Ca 2+ and / or Mg 2+ is 2 to 12%, and / or Ln 3+ 0 to 5% and / or Na + and / or Li + and / or K + 4. The fluorophosphate optical glass according to claim 1, wherein the content of said fluorophosphate is 0 to 5%.

6. Ba 2+ / Ca 2+ is 0.12 to 0.15, and / or Ba 2+ / (Ca 2+ + Mg 2+ ) is 0.1 to 0.12, and / or O 2- / F - 4. The fluorophosphate optical glass according to claim 1, wherein m is 0.105 to 0.

2.

7. P 5+ and / or Al 3+ 30 to 35%, and / or Ba 2+ and / or Sr 2+ 15 to 20%, and / or Ca 2+ and / or Mg 2+ is 5 to 10%, and / or Ln 3+ 0.5 to 3% and / or Na + 0.5 to 2% and / or Li + and / or K +4. The fluorophosphate optical glass according to claim 1, wherein the content of said fluorophosphate is 0 to 2%.

8. O 2- / F - 4. The fluorophosphate optical glass according to claim 1, wherein the value of is 0.11 to 0.

18.

9. O 2- / F - 4. The fluorophosphate optical glass according to claim 1, wherein the value of is 0.11 to 0.

15.

10. Y 3+ is 0 to 5%, preferably 0 to 4%, more preferably 0.5 to 3%, and La 3+ is 0 to 5%, preferably 0 to 3%, more preferably 0 to 1%, and Gd 3+ is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%, and Yb 3+ 4. The fluorophosphate optical glass according to claim 1, wherein the content of 0 to 5%, preferably 0 to 3%, more preferably 0 to 1%.

11. F - The content is 85 to 92%, more preferably 87 to 91%, and O 2- 4. The fluorophosphate optical glass according to claim 1, wherein the content is 8 to 15%, and more preferably 9 to 13%.

12. The thermal expansion coefficient of glass (α 20℃~120℃ ) is 155 x 10 -7 / K or less, and the density (ρ) is 3.53 g / cm 3 or less, and the degree of foam is grade B or more, preferably grade A or more, and more preferably grade A. 0 or more, and water resistance (D W 4. The fluorophosphate optical glass according to claim 1, wherein the fluorophosphate optical glass has a refractive index of 1 or higher.

13. An optical preform made from the fluorophosphate optical glass according to any one of claims 1 to 12.

14. An optical element, characterized in that it is produced from the fluorophosphate optical glass according to any one of claims 1 to 12 or from the optical preform according to claim 13.

15. An optical instrument made from the optical element according to claim 14.

Citation Information

Patent Citations

  • Fluorophosphate glass, glass material for press-molding, optical element blank, optical element and methods for manufacturing the same

    JP2009256167A

  • Fluorophosphate glass, preform for precision press-molding, optical element blank and optical element, and methods for manufacturing the same

    JP2009256168A

  • Fluorophosphate glass, glass base material for press forming, optical element blank, optical element and method of producing them

    JP2010059021A

  • Cullet raw material, fluorophosphate glass, glass base material for press forming, optical element blank, optical element and method of producing them

    JP2010059022A

  • Optical glass, preform for press forming, optical element, and processes for producing these

    WO2008111439A1