Semiconductive composition and power cable

A semiconducting composition with propylene-based resin and controlled viscosities addresses the uneven diameter issue in power cables, ensuring uniform insulation and stable extrusion, thus enhancing cable performance.

JP7582511B2Active Publication Date: 2024-11-13SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023563904
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-08-26
Filing Date
2023-04-20
Publication Date
2024-11-13
Estimated Expiration
2043-04-20

Smart Images

  • Figure 0007582511000003
    Figure 0007582511000003
  • Figure 0007582511000001
    Figure 0007582511000001
  • Figure 0007582511000002
    Figure 0007582511000002
Patent Text Reader

Abstract

A semiconductive composition for forming a semiconducting layer in a power cable, wherein the semiconductive composition contains carbon black and a resin component including a propylene resin and at least one of a rubber material and an elastomer, the rubber material and elastomer have at least two units from among ethylene, propylene, butylene, hexene, isoprene, octene, and styrene, the viscosity at a high shear rate at a temperature of 190°C and a shear rate of 100 s-1 is 1,000-5,000 Pa∙s inclusive, and the viscosity at a low shear rate at a temperature of 190°C and a shear rate of 1 s-1 is 100,000-1,000,000 Pa∙s inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority based on Japanese application "Patent Application No. 2022-134933" filed on August 26, 2022, and incorporates all of the contents of the above-mentioned Japanese application by reference.

[0002] The present disclosure relates to semiconductive compositions and power cables. [Background technology]

[0003] Cross-linked polyethylene has excellent insulating properties and has therefore been widely used as a resin component constituting the insulating layer in power cables and the like (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-69611 Summary of the Invention

[0005] According to one aspect of the present disclosure, A semiconductive composition for forming a semiconductive layer in a power cable, comprising: a resin component including a propylene-based resin and at least one of a rubber material and an elastomer; Carbon black, The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less. A semiconductive composition is provided. [Brief description of the drawings]

[0006] [Figure 1] FIG. 2 is a schematic cross-sectional view perpendicular to the axial direction of a DC power cable according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] (Problem to be solved by the invention) However, cross-linked polyethylene that has deteriorated over time cannot be recycled and must be incinerated, raising concerns about its impact on the environment.

[0008] In recent years, therefore, resins containing propylene (hereinafter also referred to as "propylene-based resins") have been attracting attention as resin components forming the insulating layer of power cables. Even if the propylene-based resin is not cross-linked, it can satisfy the insulating properties required for a power cable. In other words, it can achieve both insulating properties and recyclability. Furthermore, the use of propylene-based resins can improve the handling, processability, and ease of manufacture.

[0009] However, according to the study by the present inventors, it was confirmed that the outer diameter of the power cable tends to be non-uniform in the cross section and longitudinal direction of the power cable when a propylene-based resin is used, compared with the case where polyethylene is used for cross-linking. In particular, it was confirmed that the outer diameter tends to be non-uniform when the insulating layer is formed to be relatively thick with respect to the conductor, and the outer diameter of the power cable is increased.

[0010] An object of the present disclosure is to provide a technique for improving the uniformity of the outer diameter of a power cable when a propylene-based resin is used as the resin component.

[0011] (Effects of the present disclosure) According to the present disclosure, the uniformity of the outer diameter of a power cable can be improved when a propylene-based resin is used as the resin component.

[0012] <Description of the embodiments of the present disclosure> (Findings Obtained by the Inventors) First, the findings of the inventors will be outlined.

[0013] As described above, when a propylene-based resin is used as a covering material for a power cable, the outer diameter is more likely to vary than in the case of cross-linked polyethylene because the propylene-based resin is not cross-linked.

[0014] In general, in the manufacture of a power cable, first, a coating material for forming an inner semiconductive layer, a coating material for forming an insulating layer, and a coating material for forming an outer semiconductive layer are simultaneously extruded so as to be laminated on the outer circumference of a conductor. When these coating materials are crosslinked, for example, a cable is introduced into a crosslinking tube and heated in a high-temperature environment. After crosslinking, the cable is introduced into, for example, a cooling tank, and the coating materials such as the inner semiconductive layer, the insulating layer, and the outer semiconductive layer are cooled. In this case, the viscosity of the coating material increases during the crosslinking process, so that the coating material is easily maintained in the extruded shape, and the shape can be fixed as it is by cooling. In other words, crosslinking can suppress sagging due to the flow of the coating material and the associated fluctuation in the outer diameter of the power cable.

[0015] In contrast, when a propylene-based resin is used as the coating material, the coating material is extruded and then cooled because no crosslinking treatment is performed. At this time, the laminated coating material is gradually cooled from the surface side to the inside. Therefore, the surface side of the laminated coating material is cooled to fix its shape, while the inside may be in a high-temperature melt-flowable state. Moreover, since no crosslinking treatment is performed, the viscosity of the coating material cannot be increased. As a result, the coating material may sag under its own weight before the inside of the coating material is cooled and the shape is fixed. Due to this sagging, the thickness of the coating layer may become uneven in the circumferential direction in the cross section of the power cable, and the thickness may also become uneven in the longitudinal direction of the power cable. For example, when the power cable is transported horizontally using a horizontal extruder, the coating material may sag downward in the cross section of the power cable, and when the power cable is transported vertically using a vertical extruder, the coating material may sag downward in the longitudinal direction of the power cable. If the thickness of the insulating coating is non-uniform in the circumferential direction or longitudinal direction of the cross section, there will be places where the insulating properties are locally low, and the desired insulating properties may not be achieved.

[0016] The sagging of the covering material is more likely to occur the thicker the extrusion is, and the greater the thickness of the insulating layer and the greater the ratio of the thickness of the insulating layer to the outer diameter of the conductor, the more noticeable the sagging becomes.

[0017] For this reason, the present inventors have studied a method for suppressing sagging of the insulating layer, which has a large effect on the outer diameter fluctuation, among the coating layers including the internal semiconductive layer, the insulating layer, and the external semiconductive layer. Then, they focused on the viscosity of the semiconductive composition forming the external semiconductive layer. This is because by setting the viscosity of the semiconductive composition high, sagging due to the flow of the resin composition forming the insulating layer disposed inside can be suppressed and the shape can be maintained. On the other hand, the semiconductive composition is also required to have extrusion moldability, and is required to have a viscosity that allows it to be stably extruded at a constant thickness.

[0018] In general, the viscosity of a resin varies greatly depending on the shear rate, and tends to be low at high shear rates and high at low shear rates. In the production of a power cable, the semiconductive composition tends to have a high shear rate and low viscosity at the stage of melt-kneading and extrusion. On the other hand, the shear rate tends to be low and the viscosity tends to be high at the stage after extrusion and before cooling. In addition, when carbon black is further blended into the semiconductive composition, the viscosity at high shear rates and low shear rates tends to be high overall.

[0019] Based on this, the inventors of the present invention have investigated the viscosity of the semiconductive composition at both high and low shear rates, and have found that by adjusting each viscosity to fall within a predetermined range, it is possible to achieve both extrusion moldability and suppression of sagging during cooling until the shape is fixed. It has been found that such a semiconductive composition can improve the uniformity of the outer diameter of a power cable.

[0020] The present disclosure has been made based on the above findings.

[0021] (Embodiments of the present disclosure) Next, embodiments of the present disclosure will be listed and described.

[0022] [1] A semiconductive composition according to one embodiment of the present disclosure comprises: A semiconductive composition for forming a semiconductive layer in a power cable, comprising: a resin component including a propylene-based resin and at least one of a rubber material and an elastomer; Carbon black, The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less. With this configuration, the uniformity of the outer diameter of the power cable can be improved.

[0023] [2] A power cable according to one embodiment of the present disclosure includes: A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; an outer semiconductive layer formed from a semiconductive composition and covering the outer periphery of the insulating layer; The semiconductive composition is a resin component including a propylene-based resin and at least one of a rubber material and an elastomer; Carbon black, The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less. This configuration can improve the uniformity of the outer diameter.

[0024] [3] The power cable according to [2] above, The content of the carbon black is 10 parts by mass or more and 100 parts by mass or less with respect to 100 parts by mass of the resin component. According to this configuration, the uniformity of the outer diameter of the power cable can be further improved, and the electric field can be made more uniform.

[0025] [4] The power cable according to [2] or [3] above, The heat of fusion of the resin component is 55 J / g or more and 90 J / g or less. According to this configuration, the uniformity of the outer diameter can be improved more reliably.

[0026] [5] The power cable according to [2] or [3] above, The melting point of the resin component is 140°C or higher and 170°C or lower. According to this configuration, the uniformity of the outer diameter can be improved more reliably.

[0027] [6] The power cable according to [2] or [3] above, In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less. According to this configuration, it is possible to improve the uniformity of the outer diameter in the outer circumferential direction in the cross section of the power cable.

[0028] [7] The power cable according to [2] or [3] above, In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less. With this configuration, the uniformity of the outer diameter in the longitudinal direction of the power cable can be improved.

[0029] [8] The power cable according to [2] or [3] above, The thickness of the outer semiconductive layer is 0.5 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less. According to this configuration, even when the insulating layer is formed to be relatively thick compared to the outer diameter of the conductor to increase the outer diameter of the power cable, the uniformity of the outer diameter can be maintained.

[0030] DETAILED DESCRIPTION OF EMBODIMENTS OF THE DISCLOSURE Next, an embodiment of the present disclosure will be described below with reference to the drawings. Note that the present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0031] (One embodiment of the present disclosure) (1) Semiconductive composition The semiconductive composition of this embodiment can be used as a material for forming a semiconductive layer of a power cable. It may be used in the semiconductive layer, the outer semiconductive layer, or the inner semiconductive layer. The semiconductive composition contains a resin component containing a propylene-based resin and at least one of a rubber material and an elastomer, and carbon black, and the viscosity at high shear rate and low shear rate is adjusted to be within a predetermined range by mixing these components. Specifically, the viscosity of the semiconductive composition is set to be 0.01% at a temperature of 190°C and a shear rate of 100 s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less.

[0032] The components of the semiconductive composition, the composition thereof, and physical properties such as the viscosity of the resin composition will be described in detail below.

[0033] (1-1) Propylene-based resin The propylene-based resin is a base polymer of the semiconductive composition. Examples of the propylene-based resin include a propylene homopolymer (hereinafter also referred to as homo PP) and a propylene random polymer (hereinafter also referred to as random PP). The homopolymer contains a propylene unit, and the random polymer contains a propylene unit and an ethylene unit. From the viewpoint of obtaining higher flexibility in the semiconductive layer, the propylene-based resin may be a random PP. The random PP contains an ethylene unit and has a lower amount of crystals than the homopolymer, so that it is difficult to generate coarse crystals during cooling, and the flexibility of the semiconductive layer can be further improved.

[0034] The content of the ethylene unit in the random PP may be, for example, 0.5% by mass or more and 15% by mass or less. By making the content of the ethylene unit 0.5% by mass or more, it is easy to suppress the generation of coarse crystals, and the flexibility of the semiconductive layer can be maintained at a high level. On the other hand, by making the content of the ethylene unit 15% by mass or less, it is possible to suppress the decrease in the melting point and to stably realize the use in a non-crosslinked or slightly crosslinked state.

[0035] The stereoregularity of the propylene resin may be isotactic, syndiotactic, or atactic. The stereoregularity is not particularly limited, but may be isotactic. When the stereoregularity is isotactic, the melting point of the semiconductive composition can be suppressed from decreasing. As a result, the semiconductive composition can be used stably in a non-crosslinked or slightly crosslinked state.

[0036] The viscosity of the propylene-based resin at high shear rate and low shear rate is not particularly limited. The viscosity at high shear rate may be 100 Pa·s or more and 6000 Pa·s or less. The viscosity at low shear rate may be 500 Pa·s to 50000 Pa·s or less. By having such a viscosity, it is easy to adjust the viscosity to a predetermined value in the semiconductive composition. By setting the viscosity of the propylene-based resin as the base polymer in the above range, it becomes possible to reliably adjust the viscosity at each shear rate in the semiconductive composition to the above range when mixed with an elastomer or the like.

[0037] As the propylene-based resin, one having a viscosity within a predetermined range at high shear rate or low shear rate may be used alone, or two or more different viscosities may be used in combination. From the viewpoint of adjusting the viscosity of the resin composition to a predetermined range, two or more types may be used in combination.

[0038] As described later, the resin components such as the propylene-based resin have different possible viscosity curves depending on the physical properties such as the melting point, heat of fusion, molecular weight distribution, etc. In this embodiment, from the viewpoint of adjusting the viscosity of the semiconductive composition to a predetermined range, the physical properties of the propylene-based resin may be set as follows.

[0039] The melting point of the propylene-based resin is not particularly limited, but may be 160°C or more and 175°C or less if it is a propylene homopolymer (homo PP), and may be 140°C or more and 150°C or less if it is a propylene random polymer (random PP). Such a propylene-based resin makes it easy to adjust the viscosity of the semiconductive composition to a predetermined range. Moreover, the melting point of the semiconductive composition can be increased to improve the heat resistance temperature of the semiconductive layer, etc. This allows the semiconductive layer to stably maintain high performance in a high-temperature environment even if it is not crosslinked.

[0040] The heat of fusion of the propylene-based resin is not particularly limited, but may be 100 J / g or more and 120 J / g or less if it is a homo PP, or 90 J / g or more and 105 J / g or less if it is a random PP. Such a propylene-based resin makes it easy to adjust the viscosity of the semiconductive composition to a predetermined range, and also improves the heat resistance temperature of the semiconductive layer, thereby enabling various properties to be stably maintained even in a high-temperature environment.

[0041] In this specification, the melting point and heat of fusion are measured as follows. First, the sample is subjected to differential scanning calorimetry (DSC) in accordance with, for example, JIS-K-7121 (1987). Specifically, in a DSC device, the temperature is raised from room temperature (normal temperature, for example, 27°C) to 220°C at a rate of 10°C / min. In this way, a DSC curve is obtained by plotting the amount of heat absorbed (heat flow) per unit time against the temperature. At this time, the temperature at which the amount of heat absorbed per unit time in the sample is maximized (peak) is defined as the "melting point (melting peak temperature)". In addition, at this time, it is assumed that all of the heat absorbed by the sample is caused by the resin component, and the value (J / g) obtained by dividing the amount of heat absorbed by the sample from room temperature to 220°C by the mass (g) of the entire resin component in the sample is defined as the "heat of fusion". The crystallinity (%) of the sample can be calculated based on the heat of fusion of the sample and the theoretical value of the heat of fusion of a perfect crystal.

[0042] Propylene-based resins have a certain molecular weight distribution, and the wider the molecular weight distribution, that is, the larger the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) in the molecular weight distribution, the larger the difference between the viscosity at high shear rate and the viscosity at low shear rate tends to be. From the viewpoint of adjusting the viscosity at each shear rate in the semiconductive composition to within the above range, Mw / Mn may be 3.0 or more and 8.0 or less, or 3.5 or more and 7.0 or less. In addition, the number average molecular weight Mn may be, for example, 60,000 or more and 150,000 or less. In addition, the weight average molecular weight Mw may be, for example, 210,000 or more and 1,000,000 or less.

[0043] (1-2) Rubber materials / elastomers The rubber material or elastomer controls the crystal growth of the propylene-based resin in the semiconductive composition and imparts flexibility to the semiconductive layer. Although the rubber material or elastomer may change the viscosity of the semiconductive composition at each shear rate when mixed with the propylene-based resin, the rubber material or elastomer can impart a predetermined flexibility to the semiconductive layer by mixing the rubber material or elastomer so as to obtain a predetermined viscosity range. The rubber material or elastomer of this embodiment contains at least two of ethylene, propylene, butene, hexene, isoprene, octene, and styrene.

[0044] The viscosities of the rubber material or elastomer at high shear rate and low shear rate are not particularly limited. The viscosity at high shear rate may be 300 Pa·s or more and 7000 Pa·s or less. The viscosity at low shear rate may be 4000 Pa·s or more and 80000 Pa·s or less. Alternatively, the viscosity at high shear rate of the rubber material may be 500 Pa·s or more and 5000 Pa·s or less, and the viscosity at low shear rate may be 10000 Pa·s or more and 70000 Pa·s or less. The viscosity at high shear rate of the elastomer may be 1000 Pa·s or more and 6000 Pa·s or less, and the viscosity at low shear rate may be 5000 Pa·s or more and 50000 Pa·s or less. According to the rubber material or elastomer having such a viscosity, it is easy to adjust each viscosity of the semiconductive composition to a desired range when mixed with the propylene-based resin.

[0045] The melting points of rubber materials and elastomers are not particularly limited. Rubber materials generally do not have a melting point because no endothermic peak is detected in DSC measurements. Elastomers do not have to have a melting point, and even if they do have a melting point, the melting point may be 100°C or lower.

[0046] The heat of fusion of the rubber material or elastomer is not particularly limited. The heat of fusion of the rubber material is not included because the melting point cannot be measured. The heat of fusion of the elastomer may be 50 J / g or less, or 30 J / g or less.

[0047] Specifically, the rubber material may be a copolymer of at least two of ethylene, propylene, butene, hexene, and octene.

[0048] The rubber material may be a copolymer containing propylene from the viewpoint of compatibility with propylene-based resins. As the copolymer containing propylene, for example, ethylene propylene rubber (EPR) can be used.

[0049] The ethylene content of the EPR may be, for example, 20% by mass or more, 40% by mass or more, or 55% by mass or more. If the ethylene content is less than 20% by mass, the crystallization of the propylene-based resin may not be sufficiently controlled. In contrast, by setting the ethylene content to 20% by mass or more, it is possible to obtain the softening effect of the EPR while sufficiently controlling the crystallization of the propylene-based resin by the EPR. Furthermore, by setting the ethylene content to 40% by mass or more, or 55% by mass or more, it is possible to more stably control the crystallization. The density of VLDPE is, for example, 0.855 g / cm 3 More than 0.890g / cm 3 The following is the result.

[0050] On the other hand, the rubber material may be, for example, a copolymer that does not contain propylene. As a copolymer that does not contain propylene, for example, very low density polyethylene (VLDPE) can be used from the viewpoint of easy availability. Examples of VLDPE include PE composed of ethylene and 1-butene, and PE composed of ethylene and 1-octene. By using a copolymer that does not contain propylene, the crystallization of the propylene-based resin can be stably controlled.

[0051] As the elastomer, for example, a styrene-based thermoplastic elastomer containing styrene as a hard segment and at least one of ethylene, propylene, butene, and isoprene as a soft segment can be used. Like rubber materials, the styrene-based thermoplastic elastomer is a component that is dispersed in the semiconductive composition to control the crystal growth of the propylene-based resin, impart flexibility to the semiconductive layer, and contribute to adjusting the viscosity of the semiconductive composition. Furthermore, the styrene-based thermoplastic elastomer suppresses the occurrence of mechanical stress cracks in the semiconductive layer, thereby contributing to improving the water tree resistance of the semiconductive layer.

[0052] Examples of styrene-based thermoplastic elastomers include styrene-butadiene-styrene block copolymers (SBS), hydrogenated styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene copolymers (SIS), hydrogenated styrene-isoprene-styrene copolymers, hydrogenated styrene-butadiene rubber, hydrogenated styrene-isoprene rubber, styrene-ethylene-butylene olefin crystalline block copolymers, etc. Two or more of these may be used in combination.

[0053] In this case, "hydrogenation" means that hydrogen has been added to the double bond. For example, "hydrogenated styrene butadiene styrene block copolymer" means a polymer in which hydrogen has been added to the double bond of a styrene butadiene styrene block copolymer. No hydrogen has been added to the double bond of the aromatic ring of styrene. "Hydrogenated styrene butadiene styrene block copolymer" can be rephrased as styrene ethylene butylene styrene block copolymer (SEBS).

[0054] The styrene-based thermoplastic elastomer may not contain a double bond in its chemical structure. If a double bond is used, the resin component may be thermally deteriorated during molding of the semiconductive composition, which may deteriorate the properties of the resulting semiconductive layer. In this regard, a material that does not contain a double bond has high resistance to thermal deterioration, and therefore the properties of the semiconductive layer can be maintained at a high level.

[0055] The styrene content in the styrene-based thermoplastic elastomer is not particularly limited, but may be from 5% by mass to 35% by mass from the viewpoints of controlling the crystal growth of the propylene-based resin and softening the semiconductive layer.

[0056] (1-3) Carbon black Carbon black is added to and mixed with a resin component to impart electrical conductivity to the resin component. For example, furnace carbon black or acetylene carbon black may be used as the carbon black. Here, furnace carbon black refers to carbon black produced by burning oil or the like. Acetylene carbon black refers to carbon black produced by thermally decomposing acetylene as a raw material.

[0057] The average particle size of carbon black is not particularly limited, and may be appropriately set within a range that allows the carbon black to be dispersed appropriately in the semiconductive layer and obtain a desired conductivity. For example, the average particle size may be 35 nm or more and 100 nm or less. The average particle size here indicates the particle size at 50% of the cumulative value in the particle size distribution obtained by particle size measurement using a laser diffraction / scattering method.

[0058] (1-4) Other additives The semiconductive composition may contain, in addition to the above-mentioned resin component and carbon blank, for example, an antioxidant, a copper inhibitor, a lubricant, and a colorant.

[0059] However, the semiconductive composition may contain a small amount of additives that function as nucleating agents for generating propylene crystals, or may not contain such additives substantially. Specifically, the amount of additives that function as nucleating agents may be less than 1 part by mass or may be 0 parts by mass, when the total amount of the resin components including the propylene-based resin and at least one of the rubber material and the elastomer is taken as 100 parts by mass. This makes it possible to suppress the occurrence of unexpected abnormal crystallization caused by the nucleating agent and to easily control the amount of crystals.

[0060] The semiconductive composition may contain an inorganic filler, but from the viewpoint of adjusting the viscosity at high shear rate and low shear rate within a predetermined range, the amount of the inorganic filler added may be small, or no inorganic filler may be added.

[0061] (1-5) Viscosity of Semiconductive Composition The semiconductive composition is formed by mixing a propylene-based resin, at least one of a rubber material and an elastomer, and carbon black. By mixing these components, the semiconductive composition is heated at a temperature of 190° C. and a shear rate of 100 s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less.

[0062] Propylene-based resin, rubber material, and elastomer each have their own unique viscosity curve. The viscosity curve is a curve with the horizontal axis representing the shear rate and the vertical axis representing the viscosity, with the viscosity decreasing as the shear rate increases. This viscosity curve has a unique shape depending on the molecular weight, molecular weight distribution, melting point, heat of fusion, etc. of the resin. Not only when the types of propylene-based resin, rubber material, and elastomer are different, but also when the physical properties such as molecular weight distribution and melting point are different even for the same propylene-based resin, the viscosity curve will also be different. Due to the difference in viscosity curve, the slope of the viscosity curve and the viscosity range that can be taken at high shear rate and low shear rate are different. In this embodiment, the viscosity at each shear rate is adjusted by mixing propylene-based resin, rubber material, and elastomer with different viscosity curves. Moreover, the viscosity curve of the semiconductive composition is controlled by adding carbon black to the resin component, and the viscosity at each shear rate is adjusted.

[0063] In the semiconductive composition, if the viscosity at high shear rate is less than 1000 Pa·s, the molten semiconductive composition may not be extruded stably with a uniform thickness while maintaining its shape. On the other hand, if the viscosity at high shear rate exceeds 5000 Pa·s, the pressure when extruding the semiconductive composition increases, and the extrusion amount is not stable, so that the semiconductive composition may not be extruded with a uniform thickness. In this regard, by adjusting the viscosity at high shear rate to within the range of 1000 Pa·s to 5000 Pa·s, the semiconductive composition can be extruded with a uniform thickness while suppressing the flow of the coating material for forming the insulating layer and maintaining its shape. The viscosity at high shear rate may be 1000 Pa·s to 3000 Pa·s.

[0064] If the viscosity at low shear rate is less than 100,000 Pa·s, the flow (sagging) of the covering material for forming the insulating layer during the production of the power cable cannot be suppressed, and the outer diameter tends to fluctuate. On the other hand, if the viscosity at low shear rate exceeds 1,000,000 Pa·s, the viscosity at high shear rate also increases accordingly, so that the extrusion amount of the semiconductive composition becomes unstable as described above, and the semiconductive layer may not be formed with a uniform thickness. In this regard, by adjusting the viscosity at low shear rate to within the range of 100,000 Pa·s to 1,000,000 Pa·s, the sagging of the extruded semiconductive composition can be suppressed, and the uniformity of the outer diameter of the power cable can be improved. The viscosity at low shear rate may be 100,000 Pa·s to 300,000 Pa·s.

[0065] The ratio of the viscosity at high shear rate to the viscosity at low shear rate is not particularly limited, but when the viscosity at high shear rate is A and the viscosity at low shear rate is B, B / A may be 30 or more and 1000 or less. The larger this ratio is, the lower the pressure at which the molten semiconductive composition can be extruded, and the more the sagging of the material forming the insulating layer can be suppressed during the production of the power cable.

[0066] The viscosities at high and low shear rates were measured by the procedure shown in the Examples section below.

[0067] (1-6) Melting point and heat of fusion of semiconductive composition The melting point and heat of fusion of the semiconductive composition vary depending on the amount of each of the propylene-based resin, rubber material, and elastomer mixed as the resin components. In other words, the melting point and the like are indicators of the ratio (composition) of each component. The melting point and heat of fusion of the semiconductive composition are substantially the same as those of the resin components excluding carbon black.

[0068] Propylene-based resins have a relatively high melting point, whereas rubber materials and elastomers have no melting point, or if they do, the melting point is low. Propylene-based resins are highly crystalline and have a high heat of fusion, whereas rubber materials and elastomers are low crystalline or amorphous and have a low heat of fusion. Therefore, the melting point and heat of fusion of the resin components in the semiconductive composition tend to be lower than the melting point and heat of fusion inherent to the propylene-based resin.

[0069] The melting point and heat of fusion of the resin components are not particularly limited, but from the viewpoint of mixing the components in an appropriate ratio and setting the viscosities at high shear rate and low shear rate within the specified ranges, the melting points and heat of fusion may be in the following ranges, respectively.

[0070] Specifically, the melting point of the resin component may be 158° C. or more and 168° C. or less if the propylene-based resin contains homo-PP, or 140° C. or more and 150° C. or less if the propylene-based resin contains random-PP.

[0071] The heat of fusion of the resin component may be 75 J / g or more and 110 J / g or less if the propylene-based resin contains homo-PP, or 60 J / g or more and 100 J / g or less if the propylene-based resin contains random PP.

[0072] By mixing the propylene-based resin, rubber material, and elastomer in a specified ratio so that at least one of the melting point and heat of fusion of the resin components falls within the above range, it is possible to easily adjust the viscosity at high shear rate and low shear rate within the specified range.

[0073] (1-7) Resin composition The ratio (composition) of each component in the semiconductive composition may be appropriately adjusted according to the type of propylene-based resin, rubber material, and elastomer so that the viscosity at high shear rate and low shear rate are within the respective predetermined ranges. From the viewpoint of more reliably adjusting the viscosity to the predetermined range, each component may be mixed so that the melting point and heat of fusion of the resin component are within the above-mentioned ranges. Specifically, the addition ratio of the propylene-based resin in the resin composition may be 50 mass% or more. In addition, the propylene-based resin may be used in combination with two or more components having different viscosities, melting points, and heat of fusion. The rubber material and elastomer may also be used in combination with two or more components having different physical property values.

[0074] The content of carbon black in the semiconductive composition is not particularly limited. Carbon black increases the viscosity at each shear rate when mixed with the resin component. Therefore, it is preferable to appropriately change the viscosity at each shear rate so that it falls within a predetermined range while satisfying the conductivity required for the semiconductive layer. For example, the content of carbon black may be 10 parts by mass or more and 100 parts by mass or less, or 10 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the resin component.

[0075] (2) Power cable Next, the power cable of this embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view perpendicular to the axial direction of the power cable according to this embodiment.

[0076] The power cable 10 of this embodiment is configured as a so-called solid insulated power cable. The power cable 10 of this embodiment is configured to be laid, for example, on land (in a pipe), underwater, or at the bottom of the water. The power cable 10 is used, for example, for alternating current.

[0077] Specifically, the power cable 10 includes, for example, a conductor 110 , an inner semiconductive layer 120 , an insulating layer 130 , an outer semiconductive layer 140 , a shielding layer 150 , and a sheath 160 .

[0078] (Conductor (conductive part)) The conductor 110 is formed by twisting together a plurality of conductor core wires (conductive core wires) containing, for example, pure copper, a copper alloy, aluminum, an aluminum alloy, or the like.

[0079] (internal semiconductive layer) The internal semiconductive layer 120 is provided so as to cover the outer circumference of the conductor 110. The internal semiconductive layer 120 is semiconductive and configured to suppress electric field concentration on the surface side of the conductor 110. The internal semiconductive layer 120 is formed from a semiconductive composition containing a resin component and carbon black. As the resin component, for example, at least one of ethylene-based copolymers such as ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, and ethylene-vinyl acetate copolymer, olefin-based elastomer, and propylene-based resin can be used. Also, a semiconductive composition whose viscosity at each of the above-mentioned shear rates is adjusted to a predetermined range may be used.

[0080] (insulating layer) The insulating layer 130 is provided so as to cover the outer periphery of the internal semiconductive layer 120. A propylene-based resin is preferably used as a material for forming the insulating layer 130 in terms of non-crosslinking. In addition, a resin component containing the above-mentioned propylene-based resin and at least one of a rubber material and an elastomer may be used in terms of improving the flexibility of the insulating layer 130. The insulating layer 130 is formed, for example, by extruding a resin composition containing the resin component.

[0081] (Outer semiconducting layer) The outer semiconductive layer 140 is provided so as to cover the outer periphery of the insulating layer 130. The outer semiconductive layer 140 has semiconductivity and is configured to suppress electric field concentration between the insulating layer 130 and the shielding layer 150. The outer semiconductive layer 140 is formed from a semiconductive composition whose viscosity at each of the above-mentioned shear rates is adjusted to fall within a predetermined range.

[0082] (shielding layer) The shielding layer 150 is provided so as to cover the outer periphery of the outer semiconductive layer 140. The shielding layer 150 is formed, for example, by winding a copper tape, or is formed as a wire shield in which a plurality of soft copper wires or the like are wound. Note that a tape made of a material such as a rubber-coated cloth may be wound on the inside or outside of the shielding layer 150.

[0083] (sheath) The sheath 160 is provided so as to cover the outer periphery of the shielding layer 150. The sheath 160 is made of, for example, polyvinyl chloride or polyethylene.

[0084] If the power cable 10 of this embodiment is an underwater cable or a bottom cable, it may have a metallic water-proof layer such as aluminum sheath or iron wire armor outside the shielding layer 150. On the other hand, since the power cable 10 of this embodiment has the above-mentioned water tree suppression effect, it may not have a metallic water-proof layer such as aluminum sheath outside the shielding layer 150. In other words, the power cable 10 of this embodiment may be configured with a non-completely water-proof structure.

[0085] (Specific dimensions, etc.) Specific dimensions of the power cable 10 are not particularly limited, but for example, the diameter of the conductor 110 is 5 mm or more and 60 mm or less, the thickness of the inner semiconductive layer 120 is 0.5 mm or more and 3 mm or less, the thickness of the insulating layer 130 is 3 mm or more and 35 mm or less, the thickness of the outer semiconductive layer 140 is 0.5 mm or more and 3 mm or less, the thickness of the shielding layer 150 is 0.1 mm or more and 5 mm or less, and the thickness of the sheath 160 is 1 mm or more. The outer diameter of the power cable 10 is, for example, 15 mm or more and 170 mm or less. In particular, the thickness of the outer semiconductive layer 140 may be 0.5 mm or more or may be 1 mm or more from the viewpoint of further suppressing the outer diameter fluctuation. The AC voltage applied to the power cable 10 of this embodiment is, for example, 20 kV or more.

[0086] As described above, the greater the thickness of the insulating layer 130, particularly the higher the ratio of the thickness of the insulating layer 130 to the outer diameter of the conductor 110, the easier the shape of the insulating layer 130 is to be deformed. In this regard, in the present embodiment, the outer semiconductive layer 140 is formed using a semiconductive composition whose viscosity at each shear rate is adjusted to a predetermined range, so that sagging due to flow of the insulating layer 130 is suppressed and the shape is easily maintained. Therefore, even if the insulating layer 130 is formed thicker than the outer diameter of the conductor 110 and the outer diameter of the power cable 10 is increased, the outer diameter fluctuation can be suppressed. For example, even if the thickness of the insulating layer 130 is 4 mm or more and the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 is 4 or less, the outer diameter fluctuation can be suppressed. From the viewpoint of more reliably suppressing the outer diameter fluctuation, the thickness of the insulating layer 130 may be 13 mm or less. In addition, the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 may be 4 or less. In addition, the outer diameter of the conductor 110 is 8 mm in cross-sectional area of ​​the conductor 110. 2 More than 900mm 2 The range may be as follows:

[0087] (3) Cable characteristics In this embodiment, the outer semiconductive layer 140 is formed from the above-mentioned semiconductive composition, thereby ensuring the following cable characteristics.

[0088] (Outer diameter uniformity) In the power cable 10 of the present embodiment, sagging of the insulating layer 130 is suppressed, and therefore the variation in the outer diameter is small both in the cross section and in the longitudinal direction.

[0089] The small variation in the outer diameter in the cross section means that in a cross section perpendicular to the longitudinal direction of the power cable 10, the difference between the maximum value and the minimum value of the outer diameter in the circumferential direction is small. 1 , the minor axis (minimum outer diameter) is B 1 Then, the ratio of the long diameter to the short diameter (A 1 / B 1 ) may be 1.3 or less, or may be 1.25 or less. The lower limit of the ratio is 1.

[0090] The term "small variation in the outer diameter in the longitudinal direction" means that the difference in the outer diameter between two points in a cross section of the power cable 10 spaced apart in the longitudinal direction is small. Specifically, when comparing the outer diameters at two points spaced apart by 5 m in the longitudinal direction, the minor axis at one point is A. 2 , the major axis at the other point is B 2 (A 2 2 ), the minor axis A at one point 2 The major axis B at the other point 2 Ratio (B 2 / A 2 ) may be 1.3 or less, or 1.25 or less. The lower limit of the ratio is 1.

[0091] (4) Manufacturing method of power cables Next, a method for manufacturing the power cable according to the present embodiment will be described. Hereinafter, steps are abbreviated as "S".

[0092] (S100: Coating material preparation process) First, coating materials for forming the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140 are prepared.

[0093] The semiconductive composition for forming the outer semiconductive layer 140 may be prepared as follows.

[0094] ​First, a propylene-based resin, at least one of a rubber material and an elastomer, carbon black, and other additives (antioxidants, etc.) are mixed (kneaded) by a mixer to form a mixture. At this time, the propylene-based resin, the rubber material, the elastomer, and the carbon black are mixed in a predetermined ratio so that the viscosity at high shear rate and low shear rate in the semiconductive composition is within a predetermined range. Alternatively, the propylene-based resin, the rubber material, and the elastomer are mixed so that the melting point and the heat of fusion of the resin components are within a predetermined range, and the content of the carbon black is appropriately adjusted within a range that obtains the desired semiconductivity. Examples of the mixer include an open roll, a Banbury mixer, a pressure kneader, a single-shaft mixer, and a multi-shaft mixer.

[0095] After the mixture is formed, the mixture is granulated by an extruder, thereby forming a pellet-shaped semiconductive composition that will form the outer semiconductive layer 140. Note that the steps from mixing to granulation may be performed in one step using a twin-screw extruder that has a high kneading effect.

[0096] A conventionally known semiconductive composition can be used as the semiconductive composition for forming the inner semiconductive layer 120. For example, a composition that contains a propylene-based resin and carbon black and can be used in a non-crosslinked state can be used. In addition, for example, the semiconductive composition for forming the outer semiconductive layer 140 described above may be used.

[0097] The resin composition for forming the insulating layer 130 is not particularly limited, and a conventionally known resin composition can be used. For example, a resin composition containing a propylene-based resin can be used. Also, for example, a resin composition containing the above-mentioned propylene-based resin and at least one of a rubber material and an elastomer can be used.

[0098] (S200: Conductor preparation process) On the other hand, conductor 110 is prepared by twisting together a plurality of conductor core wires.

[0099] (S300: Cable core forming process) After the covering material preparing step S100 and the conductor preparing step S200 are completed, each covering material is extruded using, for example, a three-layer co-extruder so as to cover the outer periphery of the conductor 110 to a predetermined thickness.

[0100] Specifically, for example, a semiconductive composition for forming the inner semiconductive layer is charged into extruder A, which forms the inner semiconductive layer 120, of the three-layer co-extruder.

[0101] A pellet-shaped resin composition is fed as a coating material for forming the insulating layer into extruder B which forms the insulating layer 130. The set temperature of extruder B is set to a temperature 10° C. to 50° C. higher than the desired melting point. The set temperature may be adjusted appropriately based on the linear speed and extrusion pressure.

[0102] The above-mentioned semiconductive composition is fed into extruder C which forms the outer semiconductive layer 140 .

[0103] Next, the extrudates from extruders A to C are introduced into a common head, and the inner semiconductive layer 120, the insulating layer 130, and the outer semiconductive layer 140 are simultaneously extruded from the inside to the outside around the conductor 110. At this time, the semiconductive composition for forming the outer semiconductive layer 140 can be stably extruded with a uniform thickness because its viscosity at a high shear rate is adjusted to 1000 Pa s or more and 5000 Pa s or less. This forms the extruded material that will become the cable core.

[0104] The extruded material is then cooled, for example with water, so that each coating material solidifies and its shape is fixed.

[0105] In this embodiment, the viscosity of the semiconductive composition for forming the outer semiconductive layer is adjusted to 100,000 Pa·s or more and 1,000,000 Pa·s or less at a low shear rate, so that the flow (dripping) of the coating material forming the insulating layer 130 located inside can be suppressed. Therefore, each coating material can be fixed in the shape as it is extruded. As a result, the thickness of the insulating coating formed by the inner semiconductive layer 120, the insulating layer 130, and the outer semiconductive layer 140 can be formed uniformly in both the outer direction and the longitudinal direction of the cross section of the extruded material.

[0106] Through the above cable core formation step S300, a cable core composed of the conductor 110, the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140 is formed.

[0107] (S400: Shielding layer formation process) Once the cable core is formed, a shielding layer 150 is formed on the outside of the outer semiconducting layer 140, for example by wrapping copper tape around it.

[0108] (S500: Sheath forming process) After the shielding layer 150 is formed, vinyl chloride is put into an extruder and extruded to form a sheath 160 around the outer periphery of the shielding layer 150 .

[0109] In this manner, the power cable 10 is manufactured as a solid insulated power cable.

[0110] (5) Summary of this embodiment According to this embodiment, one or more of the following advantages are achieved.

[0111] (a) The semiconductive composition of this embodiment has a viscosity of 1000 Pa·s to 5000 Pa·s at a high shear rate. This allows the semiconductive composition to be stably extruded with a uniform thickness while maintaining the extrusion shape when melted and extruded. Also, the viscosity of the semiconductive composition at a low shear rate is 100,000 Pa·s to 1,000,000 Pa·s. This allows the semiconductive composition to press down the coating material of the insulating layer 130 when extruded onto the outer periphery of the coating material that forms the insulating layer 130. As a result, sagging due to the weight of the coating material itself is suppressed, and the insulating layer 130 can be maintained in the extrusion shape. In other words, the insulating layer 130 can be easily fixed in the extrusion shape. In this way, the semiconductive composition of this embodiment has a suitable viscosity when melted and extruded, thereby obtaining the desired extrusion moldability, while having a relatively high viscosity after extrusion, thereby making it difficult to flow and maintaining the extrusion shape.

[0112] (b) In the power cable 10 of this embodiment, by forming the outer semiconductive layer 140 using the above-mentioned semiconductive composition, it is possible to make the outer diameter uniform in both the circumferential direction and the longitudinal direction of the cross section of the power cable 10. That is, it is possible to reduce the variation in the outer diameter in the cross section and the longitudinal direction of the power cable 10. Specifically, in the cross section of the power cable 10, the ratio of the maximum outer diameter (major axis) to the minimum outer diameter (minor axis) in the circumferential direction can be set to 1.3 or less. Furthermore, in two cross sections spaced apart in the longitudinal direction of the power cable 10, the ratio of the major axis at one point to the minor axis at the other point can be set to 1.3 or less.

[0113] (c) The semiconductive composition contains at least one of a rubber material and an elastomer together with the propylene-based resin, which can suppress excessive crystal growth of the propylene-based resin during the process of cooling from a molten state, thereby making it possible to obtain a desired balance between electrical conductivity and flexibility at a high level in the outer semiconductive layer 140.

[0114] (d) In the semiconductive composition, the carbon black content may be 10 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the resin component. By setting the content in this range, the viscosity of the semiconductive composition at each shear rate can be more reliably adjusted to a predetermined range, while a predetermined semiconductivity can be obtained. As a result, the fluctuation in the outer diameter of the power cable 10 can be more reliably suppressed, and the electric field in the power cable 10 can be more uniformly suppressed to suppress partial discharge.

[0115] (e) In the semiconductive composition, the melting point of the resin component may be 140°C to 150°C if it contains random PP, and 158°C to 168°C if it contains homo PP. The heat of fusion of the resin component may be 60J / g to 100J / g if it contains random PP, and 75J / g to 110J / g if it contains homo PP. In the semiconductive composition, by having at least one of the melting point and heat of fusion of the resin component satisfy a predetermined range, the addition ratio of the propylene-based resin, the rubber material, and the elastomer can be set in an appropriate range, and the viscosity at high shear rate and low shear rate can be reliably adjusted to the above range. Moreover, the outer semiconductive layer 140 can obtain higher flexibility.

[0116] (f) Furthermore, since the semiconductive composition has a relatively large viscosity of 100,000 Pa s or more at a low shear rate, deformation of the insulating layer 130 can be suppressed even when the insulating layer 130 is formed to be thick relative to the outer diameter of the conductor 110. Specifically, by forming the outer semiconductive layer 140 to a thickness of 0.5 mm or more, it is possible to suppress the fluctuation in the outer diameter to a small value even when the insulating layer 130 is formed to be thick relative to the outer diameter of the conductor 110 so that the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 is 4 or less.

[0117] (g) Furthermore, by using the semiconductive composition, during the production of the power cable 10, it is possible to suppress fluctuations in outer diameter in the longitudinal direction, which is particularly likely to occur when a vertical extruder is used, and fluctuations in outer diameter in the circumferential direction of the cross section, which is particularly likely to occur when a horizontal extruder is used.

[0118] (h) In addition, in the power cable 10, since the semiconductive composition has a low viscosity at a low shear rate, even if the coating material forming the insulating layer 130 has a low viscosity, the shape of the insulating layer 130 can be maintained. Specifically, even if the viscosity at a low shear rate of the coating material forming the insulating layer 130 is in the range of 3000 Pa s or more, the shape of the insulating layer 130 can be maintained.

[0119] <Other embodiments of the present disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above-described embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.

[0120] In the above-described embodiment, the resin composition molded body as the insulating layer is described as being one which is mechanically mixed and extrusion molded, but the resin composition molded body may also be one which is polymerized and extrusion molded.

[0121] In the above embodiment, the case where the power cable 10 does not need to have a water-shielding layer has been described, but the present disclosure is not limited to this case. The power cable 10 may have a simple water-shielding layer because it has the above-mentioned remarkable water tree suppression effect. Specifically, the simple water-shielding layer is made of, for example, a metal laminate tape. The metal laminate tape has, for example, a metal layer made of aluminum or copper, and an adhesive layer provided on one or both sides of the metal layer. The metal laminate tape is, for example, wound by longitudinal splicing so as to surround the outer periphery of the cable core (outer periphery than the outer semiconductive layer). The water-shielding layer may be provided outside the shielding layer, or may also serve as the shielding layer. With such a configuration, the cost of the power cable 10 can be reduced.

[0122] In the above embodiment, the power cable 10 is configured to be laid on land, underwater, or on the bottom of the water, but the present disclosure is not limited to this. For example, the power cable 10 may be configured as a so-called overhead electric wire (overhead insulated electric wire). EXAMPLES

[0123] Next, examples according to the present disclosure will be described. These examples are merely examples of the present disclosure, and the present disclosure is not limited to these examples.

[0124] (1) Material First, materials A to D shown in the following Table 1 were prepared as semiconductive compositions. In preparing materials A to D, the following components were used.

[0125] As the propylene-based resin, multiple types of propylene random polymers different from each other were prepared, each having a viscosity at a high shear rate of 100 Pa·s or more and 6000 Pa·s or less, a viscosity at a low shear rate of 500 Pa·s or more and 50,000 Pa·s or less, a melting point of 140°C or more and 145°C or less, a heat of fusion of 90 J / g or more and 105 J / g or less, a ratio Mw / Mn of weight average molecular weight (Mw) to number average molecular weight (Mn) of 3.0 or more and 8.0 or less, Mn in the range of 60,000 to 150,000, and Mw in the range of 210,000 to 1,000,000.

[0126] The rubber materials prepared were several different types of EPR and VLDPE, each with a different viscosity at high shear rate of 500 Pa·s to 5000 Pa·s and a different viscosity at low shear rate of 10000 Pa·s to 70000 Pa·s, and no melting point or heat of fusion.

[0127] As elastomers, we prepared several different types of styrene-based resins with different viscosities at high shear rates in the ranges of 1000 Pa·s to 6000 Pa·s, 5000 Pa·s to 50,000 Pa·s at low shear rates, melting points in the ranges of 30°C to 80°C, and heats of fusion in the ranges of 5 J / g to 50 J / g.

[0128] The carbon black used had an average particle size of 10 nm.

[0129] In this example, the propylene-based resin was used alone or in combination with two or more types of resins whose physical properties were within the above ranges, and the rubber material or elastomer was used alone or in combination with two or more types whose physical properties were within the above ranges. The ratio of each component was appropriately changed, and a predetermined amount of carbon black was added to 100 parts by mass of these resin components, and materials A to D were prepared so that the viscosity of the obtained semiconductive composition at each shear rate was a predetermined value. Here, the addition ratio of the propylene-based resin was adjusted to be 50% by mass or more of the resin components.

[0130] [Table 1]

[0131] In Table 1, the melting points and heat of fusion of the resin components contained in materials A to D, and the viscosities at high shear rate and low shear rate of materials A to D were measured as follows.

[0132] (Melting point and heat of fusion) The melting points and heat of fusion of the resin components contained in materials A to D were determined by DSC measurement. The DSC measurement was performed in accordance with JIS-K-7121 (1987). Specifically, a PerkinElmer DSC8500 (input compensation type) was used as the DSC device. The reference sample was, for example, α-alumina. The mass of the measurement sample was 8 to 10 g. In the DSC device, the temperature was raised from room temperature (27°C) to 220°C at a rate of 10°C / min. Thus, the amount of heat absorbed (heat flow) per unit time was plotted against the temperature to obtain a DSC curve.

[0133] The temperature at which the amount of heat absorbed per unit time in each sample reached its maximum (highest peak) was taken as the "melting point." The area of ​​the region enclosed by the melting peak and the baseline in the DSC curve was calculated to determine the "heat of fusion."

[0134] (viscosity) The viscosity of materials A to D at each shear rate was measured using a rotational rheometer (Anton Paar's "MCR302") at 190 °C and a shear rate of 0.001 s -1 From 1000s -1 The shear rate was changed up to 1000 s.

[0135] (2) Preparation of a sample power cable In this example, a resin composition for forming an insulating layer was prepared separately from materials A to D as the semiconductive composition. Specifically, the propylene-based resin, rubber material, and elastomer used in the preparation of the semiconductive composition described above were appropriately mixed to prepare composition A for forming an insulating layer having a viscosity of 1000 Pa·s at a high shear rate and a viscosity of 5000 Pa·s at a low shear rate. In addition, the mixing ratio of each component was appropriately changed to prepare composition B for forming an insulating layer having a viscosity of 100 Pa·s at a high shear rate and a viscosity of 800 Pa·s at a low shear rate.

[0136] Next, compositions A and B for forming an insulating layer and materials A to D, which are semiconductive compositions, were used to prepare a sample simulating a power cable.

[0137] (Sample 1) Specifically, as shown in Table 2 below, first, the cross-sectional area is 200 mm 2A conductor (conductor diameter is about 16.0 mm) was prepared. After the conductor was prepared, the material A prepared above as the coating material for forming the internal semiconductive layer, the composition A for forming the insulating layer, and the material A prepared above as the coating material for forming the external semiconductive layer were respectively fed into extruders A to C. The extrudates from the extruders A to C were guided to a common head, and the internal semiconductive layer, the insulating layer, and the external semiconductive layer were simultaneously extruded from the inside to the outside on the outer periphery of the conductor. At this time, the thicknesses of the internal semiconductive layer, the insulating layer, and the external semiconductive layer were set to 0.5 mm, 9.0 mm, and 0.5 mm, respectively, and the insulating coating thickness was set to 10 mm. As a result, a power cable sample 1 (cable outer diameter is 36 mm) having a conductor, an internal semiconductive layer, an insulating layer, and an external semiconductive layer from the center to the periphery was manufactured. Note that when the conductor diameter is X and the outer diameter (cable outer diameter) of the power cable is Y, the ratio of the cable outer diameter to the conductor diameter (Y / X) was 1.9.

[0138] [Table 2]

[0139] (Samples 2-5) For Samples 2 to 5, as shown in Table 2, power cables were produced in the same manner as Sample 1, except that the type of semiconductive composition was changed to Material B to Material D, or the type of composition for forming the insulating layer was changed to Composition B, as appropriate. Samples 2 to 5 were obtained.

[0140] (3) Evaluation For Samples 1 to 5 produced as power cables, the uniformity of the outer diameter in the cross section of the power cable and the uniformity of the outer diameter in the longitudinal direction were evaluated.

[0141] The uniformity of the outer diameter in the cross section was evaluated as follows. Specifically, an arbitrary point in the longitudinal direction of the power cable was selected, and the outer diameter in the circumferential direction in the cross section was measured, the major axis (maximum value) and the minor axis (minimum value) were obtained, and the ratio of the major axis to the minor axis was calculated. The smaller this ratio, the smaller the variation in the outer diameter in the cross section.

[0142] The uniformity of the outer diameter in the longitudinal direction was evaluated as follows. Specifically, two points 5 m apart in the longitudinal direction of the power cable were selected, the long and short diameters were measured at each point, and the ratio of the long diameter at one point to the short diameter at the other point was calculated. The smaller this ratio, the smaller the variation in the outer diameter in the longitudinal direction.

[0143] (4) Evaluation results As shown in Table 2, it was confirmed that the use of material A or material B as the semiconductive composition in samples 1 and 2 allowed the variation in outer diameter to be reduced in both the cross-sectional and longitudinal directions. This is believed to be because material A and material B were able to suppress the sagging of composition A for forming the insulating layer, allowing the shape to be maintained.

[0144] In addition, in sample 3, material C having an excessively low viscosity at low shear rate was used, so it was confirmed that the sagging of composition A for forming the insulating layer could not be suppressed and the fluctuation in the outer diameter of the power cable could not be sufficiently suppressed.

[0145] Moreover, in Sample 4, since Material D, which has an excessively high viscosity at high shear rate, was used as the semiconductive composition, it was confirmed that the extrusion moldability was poor and the material could not be molded into a semiconductive layer.

[0146] In addition, in Sample 5, since Composition B, which has a lower viscosity at low shear rate than Composition A for forming an insulating layer, was used, it was confirmed that the fluctuation in the outer diameter of the power cable was larger than that of Sample 1.

[0147] Aspects of the present disclosure The following additional aspects of the present disclosure.

[0148] (Appendix 1) A semiconductive composition for forming a semiconductive layer in a power cable, comprising: a resin component including a propylene-based resin and at least one of a rubber material and an elastomer; Carbon black, The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less. Semiconductive composition.

[0149] (Appendix 2) A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; an outer semiconductive layer formed from a semiconductive composition and covering the outer periphery of the insulating layer; The semiconductive composition is a resin component including a propylene-based resin and at least one of a rubber material and an elastomer; Carbon black, The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 1000 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less. Power cable.

[0150] (Appendix 3) The content of the carbon black is 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the resin component. 2. A power cable as defined in claim 2.

[0151] (Appendix 4) The heat of fusion of the resin component is 55 J / g or more and 90 J / g or less. 1. A power cable as claimed in claim 2 or 3.

[0152] (Appendix 5) The melting point of the resin component is 140°C or higher and 170°C or lower. 5. The power cable according to claim 2,

[0153] (Appendix 6) In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less. 6. The power cable according to claim 2,

[0154] (Appendix 7) In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less. 7. The power cable according to claim 2,

[0155] (Appendix 8) The thickness of the outer semiconductive layer is 0.5 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less. 8. The power cable according to claim 2,

[0156] (Appendix 9) The propylene-based resin has a viscosity of 100 Pa·s or more and 6000 Pa·s or less at the high shear rate and a viscosity of 500 Pa·s to 50000 Pa·s or less at the low shear rate. 9. The power cable according to any one of appendixes 2 to 8.

[0157] (Appendix 10) The propylene-based resin has a melting point of 140° C. or more and 150° C. or less and a heat of fusion of 90 J / g or more and 105 J / g or less. 10. The power cable according to any one of appendixes 2 to 9.

[0158] (Appendix 11) The rubber material and the elastomer have a viscosity of 300 Pa·s or more and 7000 Pa·s or less at the high shear rate and a viscosity of 4000 Pa·s or more and 80000 Pa·s or less at the low shear rate. 11. The power cable according to claim 2.

[0159] (Appendix 12) The rubber material has no melting point or has a melting point of 100°C or less. Attachment 2. A power cable according to claim 1.

[0160] (Appendix 13) The rubber material has a heat of fusion of 50 J / g or less. Attachment 2. A power cable according to any one of claims 2 to 12. [Explanation of symbols]

[0161] 10 Power Cable 110 Conductor 120 Inner semiconducting layer 130 Insulating layer 140 Outer semiconducting layer 150 Shielding layer 160 Sheath

Claims

1. A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; an outer semiconductive layer formed from a semiconductive composition and covering the outer periphery of the insulating layer; The semiconductive composition is a resin component including a mixture of a propylene-based resin, a rubber material, and an elastomer; Carbon black, The propylene-based resin is at least one of a propylene homopolymer having a heat of fusion of 100 J / g or more and 120 J / g or less, and a propylene random polymer having a heat of fusion of 90 J / g or more and 105 J / g or less, the rubber material has no heat of fusion and is a copolymer of at least two of ethylene, propylene, butene, hexene, and octene; the elastomer is a styrene-based thermoplastic elastomer having a heat of fusion of 50 J / g or less and containing styrene as a hard segment and at least one of ethylene, propylene, butene, and isoprene as a soft segment; the heat of fusion of the resin component is 75 J / g or more and 110 J / g or less when the propylene-based resin contains the propylene homopolymer, and 60 J / g or more and 100 J / g or less when the propylene-based resin contains the propylene random polymer; The addition ratio of the propylene-based resin is 50% by mass or more of the resin component, Temperature: 190°C, shear rate: 100s -1 The viscosity at high shear rate is 1000 Pa·s or more and 5000 Pa·s or less at a temperature of 190°C and a shear rate of 1 s -1 The viscosity at a low shear rate is 100,000 Pa s or more and 1,000,000 Pa s or less; Power cable.

2. The content of the carbon black is 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the resin component.

2. The power cable according to claim 1.

3. The melting point of the resin component is 140° C. or higher and 170° C. or lower.

3. The power cable according to claim 1 or 2.

4. In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less.

3. The power cable according to claim 1 or 2.

5. In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less.

3. The power cable according to claim 1 or 2.

6. The thickness of the outer semiconductive layer is 0.5 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less.

3. The power cable according to claim 1 or 2.

Citation Information

Patent Citations

  • Insulating compositon for power cable

    JP1982069611A

  • Cable, and fire-resistant polymer composition

    JP1999111061A

  • Recyclable cable

    JP2004259579A

  • Cables with recyclable jackets

    JP2004510299A

  • Polyolefin compound for cable coating

    JP2018514051A