Resin composition and power cable

A resin composition with propylene resin and specific viscosity and elastic modulus ranges addresses the uneven outer diameter issue in power cables, ensuring uniformity and recyclability, and improves insulation properties.

JP7582512B2Active Publication Date: 2024-11-13SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023563983
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-08-26
Filing Date
2023-04-20
Publication Date
2024-11-13
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

Cross-linked polyethylene used in power cables deteriorates over time and cannot be recycled, leading to environmental concerns, and when replaced with propylene resin, the outer diameter of the insulating layer becomes uneven due to sagging during cooling without crosslinking, affecting insulation quality.

Method used

A resin composition comprising propylene resin and at least one of a rubber material and an elastomer, with specific viscosity and elastic modulus ranges at high and low shear rates, is used to form a uniform insulating layer, maintaining shape and preventing sagging during cooling.

Benefits of technology

The resin composition ensures a uniform outer diameter of the power cable in both cross-sectional and longitudinal directions, enhancing insulation properties and recyclability while maintaining high extrusion stability and insulation integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582512000004
    Figure 0007582512000004
  • Figure 0007582512000001
    Figure 0007582512000001
  • Figure 0007582512000002
    Figure 0007582512000002
Patent Text Reader

Abstract

A resin composition containing a propylene resin and at least one of a rubber material and an elastomer, the rubber material and elastomer having at least two units from among ethylene, propylene, butylene, hexene, isoprene, octene, and styrene, the viscosity at high shear speed at a temperature of 190°C and a shear speed of 100 s-1 being 200-5,000 Pa∙s inclusive, the viscosity at low shear speed at a temperature of 190°C and a shear speed of 1 s-1 being 7,000-50,000 Pa∙s inclusive, and the elastic modulus being 150-700 MPa inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority based on Japanese application "Patent Application No. 2022-134932" filed on August 26, 2022, and incorporates all of the contents of the above-mentioned Japanese application by reference.

[0002] The present disclosure relates to a resin composition and a power cable. [Background technology]

[0003] Cross-linked polyethylene has excellent insulating properties and has therefore been widely used as a resin component constituting the insulating layer in power cables and the like (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-69611 Summary of the Invention

[0005] According to one aspect of the present invention, A propylene-based resin, at least one of a rubber material and an elastomer; The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less, The elastic modulus is 150 MPa or more and 700 MPa or less. It is a resin composition. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view perpendicular to the axial direction of a DC power cable according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] (Problem to be solved by this disclosure) Cross-linked polyethylene that has deteriorated over time cannot be recycled and must be incinerated, which has raised concerns about its impact on the environment.

[0008] In recent years, therefore, resins containing propylene (hereinafter also referred to as "propylene-based resins") have been attracting attention as resin components constituting the insulating layer. Even if the propylene-based resin is not cross-linked, it can satisfy the insulating properties required for a power cable. In other words, it can achieve both insulating properties and recyclability. Furthermore, the use of propylene-based resins can improve handling, processability, and ease of manufacture.

[0009] However, when the inventors conducted an investigation into the use of a propylene-based resin as the resin component constituting the insulating layer, they found that the outer diameter of the insulating layer was likely to be non-uniform in the cross section and longitudinal direction of the power cable. This is because the resin component sags under its own weight during the period from when the molten resin component is extruded as the insulating layer to when it is cooled, making it impossible to maintain and fix the desired shape.

[0010] An object of the present disclosure is to provide a technique for improving the uniformity of the outer diameter of a power cable when a resin composition containing a propylene-based resin is used.

[0011] (Effects of the present disclosure) According to the present disclosure, the uniformity of the outer diameter of a power cable can be improved when a resin composition containing a propylene-based resin is used.

[0012] <Description of the embodiments of the present disclosure> (Knowledge gained by the inventors, etc.) First, the findings of the inventors will be outlined.

[0013] The non-uniformity of the outside diameter caused by the sagging of the resin component described above occurs more significantly in the case of propylene-based resin than in the case of cross-linked polyethylene.

[0014] When the insulating layer is made of cross-linked polyethylene, a resin component containing polyethylene and a cross-linking agent is extruded as the insulating layer, and then the cable is introduced into, for example, a cross-linking tube, and the resin component is heated in a high-temperature environment to cross-link. After cross-linking, the cable is introduced into, for example, a cooling tank to cool the insulating layer. In this case, the viscosity of the resin component increases during the cross-linking process, so the shape of the insulating layer is easily maintained, and the shape can be fixed by cooling. In other words, cross-linking can suppress sagging of the resin component and the associated fluctuation in the outer diameter of the power cable.

[0015] On the other hand, when the insulating layer is formed of a propylene-based resin, the resin component is extruded and then cooled because no crosslinking treatment is performed. At this time, the insulating layer is gradually cooled from the surface side to the inside. Therefore, the shape of the surface side of the insulating layer is fixed by cooling, while the inside may be in a state where it can melt and flow at a high temperature. Moreover, since no crosslinking treatment is performed, the viscosity of the resin component cannot be increased. As a result, the resin component constituting the insulating layer may sag under its own weight before the inside of the insulating layer cools and the shape is fixed. Due to this sagging, the thickness of the insulating layer may become uneven in the circumferential direction in the cross section of the power cable, and the thickness may also become uneven in the longitudinal direction of the power cable. For example, when the power cable is transported in the horizontal direction by a horizontal extruder, the resin component is likely to sag downward in the cross section of the power cable, and when the power cable is transported in the vertical direction by a vertical extruder, the resin component may sag downward in the longitudinal direction of the power cable. If the thickness of the insulating layer is non-uniform in the circumferential direction or longitudinal direction of the cross section, there will be places where the insulating properties are locally low, and the desired insulating properties may not be achieved.

[0016] The sagging of the resin component occurs more significantly as the thickness of the insulating layer increases and as the ratio of the thickness of the insulating layer to the outer diameter of the conductor increases, making the uniformity of the outer diameter of the power cable more likely to decrease.

[0017] In order to solve the above-mentioned problems, the present inventors have conducted studies focusing on the viscosity of a resin composition containing a propylene-based resin when melted.

[0018] In general, the viscosity of a resin component varies greatly depending on the shear rate, and tends to be low at high shear rates and high at low shear rates. In the production of a power cable, the shear rate is high at the stage of melt-kneading and extruding the resin composition, and the viscosity of the resin composition tends to be low. On the other hand, the shear rate is low at the stage after extrusion of the resin composition and before cooling, and the viscosity of the resin composition tends to be high.

[0019] Based on this, the present inventors have investigated the viscosity of the resin composition at both high and low shear rates, and have found that by configuring the resin composition so that each viscosity falls within a predetermined range, it is possible to achieve both extrudability and suppression of sagging during cooling until the shape is fixed. It has been found that such a resin composition can improve the uniformity of the outer diameter of the power cable.

[0020] Furthermore, power cables are required to have a certain level of insulation properties, and in order to satisfy this requirement, it has been found that it is effective to adjust the elastic modulus as well as the viscosity at each of the above-mentioned shear rates in the resin composition to fall within a certain range.

[0021] The present disclosure has been made based on the above findings.

[0022] (Embodiments of the present disclosure) Next, embodiments of the present disclosure will be listed and described.

[0023] [1] A resin composition according to one embodiment of the present disclosure, A propylene-based resin, at least one of a rubber material and an elastomer; The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less, The elastic modulus is 150 MPa or more and 700 MPa or less. According to this configuration, the resin composition can be stably extruded with a uniform thickness, and deformation of the resin composition in a molten state can be suppressed.

[0024] [2] A power cable according to another aspect of the present disclosure includes: A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; The resin composition comprises A propylene-based resin, at least one of a rubber material and an elastomer; The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; The temperature of the resin composition was 190°C and the shear rate was 100 s -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less, The elastic modulus is 150 MPa or more and 700 MPa or less. According to this configuration, it is possible to suppress the fluctuation in the outer diameter in both the circumferential direction and the longitudinal direction of the cross section of the power cable.

[0025] [3] In the power cable according to the above [2], The resin composition has a heat of fusion of 60 J / g or more and 100 J / g or less. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0026] [4] The power cable according to the above [2] or [3], The melting point of the resin composition is 140°C or higher and 150°C or lower. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0027] [5] The power cable according to any one of the above [2] to [4], The propylene-based resin has a viscosity of 100 Pa·s or more and 6000 Pa·s or less at the high shear rate, and a viscosity of 500 Pa·s to 50000 Pa·s or less at the low shear rate. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0028] [6] The power cable according to any one of the above [2] to [5], The rubber material and the elastomer have a viscosity of 300 Pa·s or more and 7000 Pa·s or less at the high shear rate, and a viscosity of 4000 Pa·s or more and 80000 Pa·s or less at the low shear rate. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0029] [7] The power cable according to any one of the above [2] to [6], In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0030] [8] The power cable according to any one of the above [2] to [7], In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less. According to this configuration, the fluctuation in the outer diameter can be more reliably suppressed.

[0031] [9] The power cable according to any one of the above [2] to [8], The thickness of the insulating layer is 4 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less. According to this configuration, even if the insulating layer is formed to be thick, the fluctuation in the outer diameter can be more reliably suppressed.

[0032] DETAILED DESCRIPTION OF EMBODIMENTS OF THE DISCLOSURE Next, an embodiment of the present disclosure will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0033] (One embodiment of the present disclosure) (1) Resin composition The resin composition of the present embodiment contains a propylene-based resin and at least one of a rubber material and an elastomer, and the viscosity and elastic modulus of the resin composition at high and low shear rates are adjusted to be within a predetermined range by mixing these components. -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at a low shear rate in the range of 7000 Pa·s to 50000 Pa·s is set to 50,000 Pa·s. The elastic modulus of the resin composition is set to 150 MPa to 700 MPa.

[0034] The components of the resin composition, the composition thereof, and physical properties such as the viscosity and elastic modulus of the resin composition will be described in detail below.

[0035] (1-1) Propylene-based resin The propylene-based resin is a base polymer of the resin composition. Examples of the propylene-based resin include propylene homopolymer (hereinafter also referred to as homo PP) and propylene random polymer (hereinafter also referred to as random PP). Homo PP contains propylene units, and random PP has propylene units and ethylene units. From the viewpoint of obtaining higher insulation in the insulating layer, the propylene-based resin may be random PP. Since random PP contains ethylene units, the amount of crystals is lower than that of homo PP, but coarse crystals are less likely to be generated during cooling, and deterioration of insulation caused by cracks due to coarse crystals can be suppressed. In other words, random PP can obtain higher insulation than homo PP.

[0036] The content of ethylene units in the random PP may be, for example, 0.5% by mass or more and 15% by mass or less. By making the content of ethylene units 0.5% by mass or more, it is easy to suppress the generation of coarse crystals, and the insulation property can be maintained at a high level. On the other hand, by making the content of ethylene units 15% by mass or less, it is possible to suppress the decrease in melting point and to stably realize the use in a non-crosslinked or slightly crosslinked state.

[0037] The stereoregularity of the propylene resin may be isotactic, syndiotactic, or atactic. The stereoregularity is not particularly limited, but may be isotactic. When the stereoregularity is isotactic, the melting point of the resin composition can be suppressed from decreasing. As a result, the resin composition can be used stably in a non-crosslinked or slightly crosslinked state.

[0038] The viscosities of the propylene-based resin at high shear rate and low shear rate are not particularly limited. The viscosity at high shear rate may be 100 Pa·s or more and 6000 Pa·s or less. The viscosity at low shear rate may be 500 Pa·s or more and 50000 Pa·s or less. By having such a viscosity, it is easy to adjust the viscosity of the resin composition to a predetermined value. By setting the viscosity of the propylene-based resin, which is the base polymer of the resin composition, within the above range, it becomes possible to reliably adjust each viscosity of the resin composition to the above range when the resin composition is prepared by mixing with an elastomer or the like.

[0039] As the propylene-based resin, one having a viscosity within a predetermined range at high shear rate or low shear rate may be used alone, or two or more different viscosities may be used in combination. From the viewpoint of adjusting the viscosity of the resin composition to a predetermined range, two or more types may be used in combination.

[0040] Moreover, the elastic modulus of the propylene-based resin is preferably 600 MPa or more and 1200 MPa or less from the viewpoint of adjusting the elastic modulus of the resin composition to a predetermined range. Here, the elastic modulus refers to the storage elastic modulus at 25°C measured by dynamic mechanical analysis (DMA). Specifically, the storage elastic modulus of the resin sample is measured while heating from -50°C to 100°C in a state where the target resin sample is stretched by 0.08% (a state where a stretching vibration with an amplitude of 0.08% is applied). At this time, the measurement frequency is 10 Hz. Also, the heating rate is 10°C / min. Then, the storage elastic modulus at 25°C is obtained.

[0041] As described later, the resin components such as the propylene-based resin have different possible viscosity curves depending on the physical properties such as the melting point, heat of fusion, molecular weight, etc. In the present embodiment, from the viewpoint of adjusting the viscosity of the resin composition to a predetermined range, the physical properties of the propylene-based resin can be set as follows.

[0042] The melting point of the propylene-based resin is not particularly limited, but may be 160°C or more and 175°C or less if it is a propylene homopolymer (homo PP), and may be 140°C or more and 150°C or less if it is a propylene random polymer (random PP). Such a propylene-based resin makes it easy to adjust the viscosity of the resin composition to a predetermined range. Moreover, the melting point of the resin composition can be increased to improve the heat resistance temperature of the insulating layer. This allows high insulation to be stably maintained in a high temperature environment even if the insulating layer is not crosslinked.

[0043] The heat of fusion of the propylene-based resin is not particularly limited, but may be 100 J / g or more and 120 J / g or less if it is a homo PP, or 90 J / g or more and 105 J / g or less if it is a random PP. Such a propylene-based resin makes it easy to adjust the viscosity of the resin composition to a predetermined range, and also improves the heat resistance temperature of the insulating layer, thereby enabling the insulating layer to stably maintain high insulating properties in a high-temperature environment.

[0044] In this specification, the melting point and heat of fusion are measured as follows. First, the sample is subjected to differential scanning calorimetry (DSC) in accordance with, for example, JIS-K-7121 (1987). Specifically, in a DSC device, the temperature is raised from room temperature (normal temperature, for example, 27°C) to 220°C at a rate of 10°C / min. In this way, a DSC curve is obtained by plotting the amount of heat absorbed (heat flow) per unit time against the temperature. At this time, the temperature at which the amount of heat absorbed per unit time in the sample is maximized (peak) is defined as the "melting point (melting peak temperature)". In addition, at this time, it is assumed that all of the heat absorbed by the sample is caused by the resin component, and the value (J / g) obtained by dividing the amount of heat absorbed by the sample from room temperature to 220°C by the mass (g) of the entire resin component in the sample is defined as the "heat of fusion". The crystallinity (%) of the sample can be calculated based on the heat of fusion of the sample and the theoretical value of the heat of fusion of a perfect crystal.

[0045] Propylene-based resins have a certain molecular weight distribution, and the wider the molecular weight distribution, that is, the larger the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) in the molecular weight distribution, the larger the difference between the viscosity at high shear rate and the viscosity at low shear rate tends to be. From the viewpoint of satisfying the above range of viscosity at each shear rate of the propylene-based resin, Mw / Mn may be 3.0 or more and 8.0 or less, or 3.5 or more and 7.0 or less. In addition, the number average molecular weight Mn may be, for example, 60,000 or more and 150,000 or less. In addition, the weight average molecular weight Mw may be, for example, 210,000 or more and 1,000,000 or less.

[0046] (1-2) Rubber materials / elastomers The rubber material or elastomer controls the crystal growth of the propylene-based resin in the resin composition and imparts flexibility to the insulating layer. Although the rubber material or elastomer may change the viscosity of the resin composition at each shear rate when mixed with the propylene-based resin, the rubber material or elastomer can impart a predetermined flexibility to the insulating layer by mixing the rubber material or elastomer so as to obtain a predetermined viscosity range. The rubber material or elastomer of this embodiment contains at least two of ethylene, propylene, butene, hexene, isoprene, octene, and styrene.

[0047] The viscosities of the rubber material or elastomer at high shear rate and low shear rate are not particularly limited. The viscosity at high shear rate may be 300 Pa·s or more and 7000 Pa·s or less. The viscosity at low shear rate may be 4000 Pa·s or more and 80000 Pa·s or less. Alternatively, the viscosity at high shear rate of the rubber material may be 500 Pa·s or more and 5000 Pa·s or less, and the viscosity at low shear rate may be 10000 Pa·s or more and 70000 Pa·s or less. The viscosity at high shear rate of the elastomer may be 1000 Pa·s or more and 6000 Pa·s or less, and the viscosity at low shear rate may be 5000 Pa·s or more and 50000 Pa·s or less. According to the rubber material or elastomer having such a viscosity, it is easy to adjust each viscosity of the resin composition to a desired range when mixed with the propylene-based resin.

[0048] The melting points of rubber materials and elastomers are not particularly limited. Rubber materials generally do not have a melting point because no endothermic peak is detected in DSC measurements. Elastomers do not have to have a melting point, and even if they do have a melting point, the melting point may be 100°C or lower.

[0049] The heat of fusion of the rubber material or elastomer is not particularly limited. The heat of fusion of the rubber material is not included because the melting point cannot be measured. The heat of fusion of the elastomer may be 50 J / g or less, or 30 J / g or less.

[0050] The elastic modulus (25°C) of the rubber material or elastomer is not particularly limited, but may be 1 MPa or more and 200 MPa or less from the viewpoint of adjusting the elastic modulus of the resin composition to a predetermined range. The elastic modulus of the rubber material or elastomer may vary greatly depending on the presence or absence of styrene. Specifically, when styrene is not contained, the elastic modulus tends to increase as the molecular weight increases, and when styrene is contained, the elastic modulus tends to decrease as the molecular weight increases.

[0051] The molecular weight distribution of rubber materials and elastomers may vary the viscosity at each shear rate, as with propylene-based resins. From the viewpoint of satisfying the viscosity range at each shear rate in rubber materials and elastomers, Mw / Mn may be 1.0 or more and 3.0 or less, or 1.0 or more and 2.5 or less. The number average molecular weight Mn may be, for example, 70,000 or more and 250,000 or less. The weight average molecular weight Mw may be, for example, 70,000 or more and 600,000 or less.

[0052] Specifically, the rubber material may be a copolymer of at least two of ethylene, propylene, butene, hexene, and octene.

[0053] The rubber material may be a copolymer containing propylene from the viewpoint of compatibility with propylene-based resins. As the copolymer containing propylene, for example, ethylene propylene rubber (EPR) can be used.

[0054] The ethylene content of the EPR may be, for example, 20% by mass or more, 40% by mass or more, or 55% by mass or more. If the ethylene content is less than 20% by mass, the crystallization of the propylene-based resin cannot be sufficiently controlled, and the insulating properties may be reduced. In contrast, by setting the ethylene content to 20% by mass or more, the crystallization of the propylene-based resin by EPR can be sufficiently controlled while obtaining the softening effect by EPR. As a result, the deterioration of the insulating properties can be suppressed. Furthermore, the ethylene content may be 40% by mass or more, or 55% by mass or more. This allows the crystallization to be more stably controlled, and the deterioration of the insulating properties can be stably suppressed.

[0055] On the other hand, the rubber material may be, for example, a copolymer that does not contain propylene. As a copolymer that does not contain propylene, for example, very low density polyethylene (VLDPE) can be used from the viewpoint of easy availability. Examples of VLDPE include PE composed of ethylene and 1-butene, and PE composed of ethylene and 1-octene. By using a copolymer that does not contain propylene, it is possible to stably control the crystallization of the propylene-based resin. The density of VLDPE is, for example, 0.855 g / cm. 3 More than 0.890g / cm 3 The following is the result.

[0056] As the elastomer, for example, a styrene-based thermoplastic elastomer containing styrene as a hard segment and at least one of ethylene, propylene, butene, and isoprene as a soft segment can be used. Like rubber materials, the styrene-based thermoplastic elastomer is a component that is dispersed in the resin composition to control the crystal growth of the propylene-based resin, impart flexibility to the insulating layer, and contribute to adjusting the viscosity of the resin composition. Furthermore, the styrene-based thermoplastic elastomer traps electrons with the aromatic ring to form a stable resonance structure, and as an elastomer, it suppresses the occurrence of mechanical stress cracks in the insulating layer, thereby contributing to improving the water tree resistance of the insulating layer.

[0057] Examples of styrene-based thermoplastic elastomers include styrene-butadiene-styrene block copolymers (SBS), hydrogenated styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene copolymers (SIS), hydrogenated styrene-isoprene-styrene copolymers, hydrogenated styrene-butadiene rubber, hydrogenated styrene-isoprene rubber, styrene-ethylene-butylene olefin crystalline block copolymers, etc. Two or more of these may be used in combination.

[0058] In this case, "hydrogenation" means that hydrogen has been added to the double bond. For example, "hydrogenated styrene butadiene styrene block copolymer" means a polymer in which hydrogen has been added to the double bond of a styrene butadiene styrene block copolymer. No hydrogen has been added to the double bond of the aromatic ring of styrene. "Hydrogenated styrene butadiene styrene block copolymer" can be rephrased as styrene ethylene butylene styrene block copolymer (SEBS).

[0059] The styrene-based thermoplastic elastomer may not contain a double bond in its chemical structure. When a double bond-containing elastomer is used, the resin component may be thermally deteriorated during molding of the resin composition, which may result in a decrease in the properties of the resulting insulating layer. In this regard, a styrene-based thermoplastic elastomer that does not contain a double bond has high resistance to thermal deterioration, and therefore can maintain the properties of the insulating layer at a high level.

[0060] The styrene content in the styrene-based thermoplastic elastomer is not particularly limited, but may be from 5% by mass to 35% by mass from the viewpoints of controlling the crystal growth of the propylene-based resin and softening the insulating layer.

[0061] (1-3) Other additives The resin composition may contain, in addition to the above-mentioned resin components, for example, an antioxidant, a copper inhibitor, a lubricant, and a colorant.

[0062] However, the resin composition may contain, for example, a small amount of additives that function as nucleating agents for generating propylene crystals, or may not contain substantially such additives. Specifically, the amount of additives that function as nucleating agents may be less than 1 part by mass or may be 0 parts by mass, when the total amount of the resin components including the propylene-based resin and at least one of the rubber material and the elastomer is taken as 100 parts by mass. This makes it possible to suppress the occurrence of unexpected abnormal crystallization caused by the nucleating agent and to easily control the amount of crystals.

[0063] The resin composition may contain an inorganic filler, but from the viewpoint of adjusting the viscosity at high shear rate and low shear rate within a predetermined range, the amount of the inorganic filler added may be small, or no inorganic filler may be added.

[0064] (1-4) Viscosity of resin composition The resin composition is formed by mixing the above-mentioned propylene-based resin with at least one of a rubber material and an elastomer, and by mixing these components, the resin composition is heated at a temperature of 190° C. and a shear rate of 100 s -1Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less.

[0065] Propylene-based resin, rubber material, and elastomer each have their own unique viscosity curve. The viscosity curve is a curve with the horizontal axis representing the shear rate and the vertical axis representing the viscosity, with the viscosity decreasing as the shear rate increases. The viscosity curve has a unique shape depending on the molecular weight, molecular weight distribution, melting point, heat of fusion, etc. of the resin component. Not only when the types of propylene-based resin, rubber material, and elastomer are different, but also when the physical properties such as molecular weight distribution and melting point are different even for the same propylene-based resin, the viscosity curve will also be different. Due to the difference in viscosity curve, the slope of the viscosity curve and the viscosity range that can be taken at high shear rate and low shear rate are different. In this embodiment, the propylene-based resin, rubber material, and elastomer with different viscosity curves are mixed to adjust the viscosity at each shear rate in the resin composition to be within a predetermined range.

[0066] In the resin composition, if the viscosity at high shear rate is less than 200 Pa·s, the molten resin composition may not be able to maintain its shape when extruded, and may not be able to be molded into an insulating layer. On the other hand, if the viscosity at high shear rate exceeds 5000 Pa·s, the pressure when extruding the resin composition increases, and the extrusion amount is not stable, so that the resin composition may not be extruded with a uniform thickness. In this regard, by adjusting the viscosity at high shear rate to within the range of 200 Pa·s to 5000 Pa·s, it becomes possible to extrude the molten resin composition with a uniform thickness while maintaining its shape. The viscosity at high shear rate may be 800 Pa·s to 3000 Pa·s.

[0067] If the viscosity at low shear rate is less than 7000 Pa·s, the extruded resin composition is likely to sag under its own weight, resulting in an uneven thickness of the insulating layer and an uneven outer diameter of the power cable. On the other hand, if the viscosity at low shear rate exceeds 50000 Pa·s, the viscosity at high shear rate also increases accordingly, so that the extrusion amount of the resin composition becomes unstable as described above, and the insulating layer may not be formed with a uniform thickness. In this regard, by adjusting the viscosity at low shear rate to within the range of 7000 Pa·s to 50000 Pa·s, the sagging of the extruded resin composition can be suppressed and the uniformity of the outer diameter of the power cable can be improved. The viscosity at low shear rate may be 10000 Pa·s to 30000 Pa·s.

[0068] The ratio of the viscosity at high shear rate to the viscosity at low shear rate is not particularly limited, but when the viscosity at high shear rate is A and the viscosity at low shear rate is B, B / A may be 10 or more and 250 or less. The larger this ratio is, the lower the pressure at which the molten resin composition can be extruded, and the better the shape of the resin composition after extrusion can be maintained.

[0069] The viscosities at high and low shear rates were measured by the procedure shown in the Examples section below.

[0070] (1-5) Elastic modulus of resin composition The resin composition is formed by mixing the above-mentioned propylene-based resin with at least one of a rubber material and an elastomer, and is configured so that the elastic modulus of the resin composition is 150 MPa or more and 700 MPa or less by mixing these components. The propylene-based resin, the rubber material, and the elastomer have different elastic moduli, and the elastic modulus of the resin composition changes depending on the amount of these components mixed. Therefore, the elastic modulus of the resin composition is an indicator of the ratio (composition) of each component. In this regard, by having the viscosity at each shear rate within the above range and the elastic modulus within the above range in the resin composition, the insulation layer can satisfy various properties required for a cable, such as uniformity of the outer diameter and insulation properties.

[0071] (1-6) Melting point and heat of fusion of resin composition The melting point and heat of fusion of the resin composition vary depending on the amounts of the propylene-based resin, rubber material, and elastomer blended, and therefore serve as indicators of the ratio (composition) of each component.

[0072] Propylene-based resins have a relatively high melting point, whereas rubber materials and elastomers have no melting point, or if they do, the melting point is low. Propylene-based resins are highly crystalline and have a high heat of fusion, whereas rubber materials and elastomers are low crystalline or amorphous and have a low heat of fusion. Therefore, the melting point and heat of fusion of the resin composition tend to be lower than the melting point and heat of fusion inherent to the propylene-based resin.

[0073] The melting point and heat of fusion of the resin composition are not particularly limited, but from the viewpoint of mixing the components in an appropriate ratio and setting the viscosities at high shear rate and low shear rate within the specified ranges, the melting point and heat of fusion may be in the following ranges, respectively.

[0074] Specifically, the melting point of the resin composition may be 158° C. or more and 168° C. or less if the propylene-based resin contains homo-PP, or 140° C. or more and 150° C. or less if the propylene-based resin contains random-PP.

[0075] The heat of fusion of the resin composition may be 75 J / g or more and 110 J / g or less if the propylene-based resin contains homo-PP, or 60 J / g or more and 100 J / g or less if the propylene-based resin contains random PP.

[0076] By mixing the propylene-based resin, rubber material, and elastomer in a specified ratio so that at least one of the melting point and heat of fusion of the resin composition falls within the above range, it is possible to adjust the viscosity and elastic modulus at high shear rate and low shear rate within a specified range.

[0077] (1-7) Resin composition The ratio (composition) of each component contained in the resin composition may be appropriately adjusted according to the type of propylene-based resin, rubber material, and elastomer so that the viscosity and elastic modulus at high shear rate and low shear rate in the resin composition are within the respective predetermined ranges. For example, each component may be mixed so that the melting point and heat of fusion of the resin composition are within the above-mentioned ranges. Specifically, the addition ratio of the propylene-based resin in the resin composition may be 50 mass% or more. In addition, the propylene-based resin may be used in combination with two or more components having different viscosities, melting points, heat of fusion, and molecular weight distributions. The rubber material and elastomer may also be used in combination with two or more components having different physical property values.

[0078] (2) Power cable Next, the power cable of this embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view perpendicular to the axial direction of the power cable according to this embodiment.

[0079] The power cable 10 of this embodiment is configured as a so-called solid insulated power cable. The power cable 10 of this embodiment is configured to be laid, for example, on land (in a pipe), underwater, or at the bottom of the water. The power cable 10 is used, for example, for alternating current.

[0080] Specifically, the power cable 10 includes, for example, a conductor 110 , an inner semiconductive layer 120 , an insulating layer 130 , an outer semiconductive layer 140 , a shielding layer 150 , and a sheath 160 .

[0081] (Conductor (conductive part)) The conductor 110 is formed by twisting together a plurality of conductor core wires (conductive core wires) containing, for example, pure copper, a copper alloy, aluminum, an aluminum alloy, or the like.

[0082] (internal semiconductive layer) The internal semiconductive layer 120 is provided so as to cover the outer periphery of the conductor 110. The internal semiconductive layer 120 has semiconductivity and is configured to suppress electric field concentration on the surface side of the conductor 110. The internal semiconductive layer 120 contains, for example, at least one of an ethylene-based copolymer such as an ethylene-ethyl acrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-butyl acrylate copolymer, and an ethylene-vinyl acetate copolymer, an olefin-based elastomer, the above-mentioned rubber material, a propylene-based resin, and the like, and conductive carbon black.

[0083] (insulating layer) The insulating layer 130 is provided so as to cover the outer periphery of the internal semiconductive layer 120, and is formed from the above-mentioned resin composition. The insulating layer 130 is formed, for example, by extruding the resin composition.

[0084] (Outer semiconducting layer) The outer semiconductive layer 140 is provided so as to cover the outer periphery of the insulating layer 130. The outer semiconductive layer 140 has semiconductivity and is configured to suppress electric field concentration between the insulating layer 130 and the shielding layer 150. The outer semiconductive layer 140 is configured, for example, from the same material as the inner semiconductive layer 120.

[0085] (shielding layer) The shielding layer 150 is provided so as to cover the outer periphery of the outer semiconductive layer 140. The shielding layer 150 is formed, for example, by winding a copper tape, or is formed as a wire shield in which a plurality of soft copper wires or the like are wound. Note that a tape made of a material such as a rubber-coated cloth may be wound on the inside or outside of the shielding layer 150.

[0086] (sheath) The sheath 160 is provided so as to cover the outer periphery of the shielding layer 150. The sheath 160 is made of, for example, polyvinyl chloride or polyethylene.

[0087] If the power cable 10 of this embodiment is an underwater cable or a bottom cable, it may have a metallic water-proof layer such as aluminum sheath or iron wire armor outside the shielding layer 150. On the other hand, since the power cable 10 of this embodiment has the above-mentioned water tree suppression effect, it may not have a metallic water-proof layer such as aluminum sheath outside the shielding layer 150. In other words, the power cable 10 of this embodiment may be configured with a non-completely water-proof structure.

[0088] (Specific dimensions, etc.) Specific dimensions of the power cable 10 are not particularly limited, but for example, the diameter of the conductor 110 is 5 mm or more and 60 mm or less, the thickness of the inner semiconductive layer 120 is 0.5 mm or more and 3 mm or less, the thickness of the insulating layer 130 is 3 mm or more and 35 mm or less, the thickness of the outer semiconductive layer 140 is 0.5 mm or more and 3 mm or less, the thickness of the shielding layer 150 is 0.1 mm or more and 5 mm or less, and the thickness of the sheath 160 is 1 mm or more. The outer diameter of the power cable 10 is, for example, 15 mm or more and 170 mm or less. The AC voltage applied to the power cable 10 of this embodiment is, for example, 20 kV or more.

[0089] As described above, the greater the thickness of the insulating layer 130, particularly the higher the ratio of the thickness of the insulating layer 130 to the outer diameter of the conductor 110, the more easily the insulating layer 130 deforms. In this regard, according to the resin composition of the present embodiment, the sagging of the insulating layer 130 is suppressed and the shape is easily maintained. Therefore, even if the insulating layer 130 is formed thicker than the outer diameter of the conductor 110 and the outer diameter of the power cable 10 is increased, deformation of the shape of the insulating layer 130 and fluctuation in the outer diameter can be suppressed. For example, the thickness of the insulating layer 130 may be 4 mm or more, and the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 may be 4 or less. From the viewpoint of suppressing the fluctuation in the outer diameter, the thickness of the insulating layer 130 may be 13 mm or less. In addition, the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 may be 4 or less. In addition, the outer diameter of the conductor 110 may be 8 mm or less in the cross-sectional area of ​​the conductor 110. 2 More than 900mm 2The range may be as follows:

[0090] (3) Cable characteristics In this embodiment, the insulating layer 130 is made of a predetermined resin composition, thereby ensuring the following cable characteristics.

[0091] (Outer diameter uniformity) In the power cable 10 of the present embodiment, sagging of the insulating layer 130 is suppressed, and therefore the variation in the outer diameter is small both in the cross section and in the longitudinal direction.

[0092] The small variation in the outer diameter in the cross section means that in a cross section perpendicular to the longitudinal direction of the power cable 10, the difference between the maximum value and the minimum value of the outer diameter in the circumferential direction is small. 1 , the minor axis (minimum outer diameter) is B 1 Then, the ratio of the long diameter to the short diameter (A 1 / B 1 ) may be 1.3 or less, or may be 1.25 or less. The lower limit of the ratio is 1.

[0093] The term "small variation in the outer diameter in the longitudinal direction" means that the difference in the outer diameter between two points in a cross section of the power cable 10 spaced apart in the longitudinal direction is small. Specifically, when comparing the outer diameters at two points spaced apart by 5 m in the longitudinal direction, the minor axis at one point is A. 2 , the major axis at the other point is B 2 (A 2 2 ), the minor axis A at one point 2 The major axis B at the other point 2 Ratio (B 2 / A 2 ) may be 1.3 or less, or 1.25 or less. The lower limit of the ratio is 1.

[0094] (Insulating) ​In the power cable 10, when the insulating layer 130 is formed to a predetermined design thickness, the insulating thickness may be locally thin, and the insulating property (apparent dielectric breakdown voltage) may be smaller than that at the predetermined thickness. In this respect, in the present embodiment, the outer diameter of the power cable 10, and particularly the thickness of the insulating layer 130, can be formed uniformly, so that the insulating property at the design thickness can be more reliably secured. Specifically, the AC breakdown field strength of the insulating layer 130 at room temperature (e.g., 27°C) is, for example, 60 kV / mm or more. More specifically, when a sample specimen with a thickness of 0.2 mm taken from the insulating layer 130 is subjected to a commercial frequency (e.g., 60 Hz) AC voltage of 10 kV for 10 minutes and then increased by 1 kV and applied for 10 minutes repeatedly at room temperature, the AC breakdown field is 60 kV / mm or more.

[0095] (4) Manufacturing method of power cables Next, a method for manufacturing the power cable according to the present embodiment will be described. Hereinafter, steps are abbreviated as "S".

[0096] (S100: Resin composition preparation step) First, a resin composition for forming the insulating layer 130 is prepared.

[0097] In this embodiment, the propylene-based resin, at least one of a rubber material and an elastomer, and other additives (antioxidants, etc.) as necessary are mixed (kneaded) by a mixer to form a mixture. Examples of the mixer include an open roll, a Banbury mixer, a pressure kneader, a single-shaft mixer, and a multi-shaft mixer.

[0098] At this time, the propylene-based resin, the rubber material, and the elastomer are mixed in a predetermined ratio so that the viscosity at high shear rate and low shear rate of the resin composition are within a predetermined range, respectively. For example, it is advisable to mix the components so that the melting point and heat of fusion of the resin composition are within a predetermined range.

[0099] After the mixture is prepared, it is granulated by an extruder, thereby forming a pellet-like resin composition that will form the insulating layer 130. Note that the steps from mixing to granulation may be performed in one step using a twin-screw extruder that has a high kneading effect.

[0100] (S200: Conductor preparation process) On the other hand, conductor 110 is prepared by twisting together a plurality of conductor core wires.

[0101] (S300: Cable core forming process (extrusion process, insulation layer forming process)) After the resin composition preparation step S100 and the conductor preparation step S200 are completed, the above-mentioned resin composition is extruded so as to cover the outer circumference of the conductor 110 to a thickness of 3 mm or more. At this time, the temperature of the resin composition is 190° C., the shear rate is 100 s -1 Since the viscosity at a high shear rate in this case is 200 Pa·s or more and 5000 Pa·s or less, the resin composition can be stably extruded to a constant thickness.

[0102] The extruded resin composition is then cooled to form the insulating layer 130. During this cooling, the temperature of the resin composition is 190° C., the shear rate is 1 s -1 Since the viscosity at low shear rate in the extrusion process is 7000 Pa·s or more and 50000 Pa·s or less, the resin composition can be prevented from flowing and dripping until the shape of the resin composition is fixed by cooling. In other words, the shape of the extruded resin composition can be fixed while being maintained. As a result, the insulating layer 130 can be formed uniformly in both the circumferential direction of the cross section and the longitudinal direction of the power cable 10.

[0103] In this embodiment, the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140 are simultaneously formed using, for example, a three-layer co-extruder.

[0104] Specifically, for example, the composition for the inner semiconductive layer is charged into extruder A, which forms the inner semiconductive layer 120, of the three-layer co-extruder.

[0105] The above-mentioned pellet-shaped resin composition is fed into extruder B which forms insulating layer 130. The set temperature of extruder B is set to a temperature which is 10° C. to 50° C. higher than the desired melting point. The set temperature may be appropriately adjusted based on the linear speed and extrusion pressure.

[0106] An outer semiconductive layer composition containing the same materials as the inner semiconductive layer resin composition charged in extruder A is charged in extruder C which forms the outer semiconductive layer 140 .

[0107] Next, the extrudates from the extruders A to C are guided to a common head, and the inner semiconductive layer 120, the insulating layer 130, and the outer semiconductive layer 140 are simultaneously extruded from the inside to the outside around the periphery of the conductor 110. This forms an extruded material that will become the cable core.

[0108] The extrusion is then cooled, for example with water.

[0109] Through the above cable core formation step S300, a cable core composed of the conductor 110, the inner semiconductive layer 120, the insulating layer 130 and the outer semiconductive layer 140 is formed.

[0110] (S400: Shielding layer formation process) Once the cable core is formed, a shielding layer 150 is formed on the outside of the outer semiconducting layer 140, for example by wrapping copper tape around it.

[0111] (S500: Sheath forming process) After the shielding layer 150 is formed, vinyl chloride is put into an extruder and extruded to form a sheath 160 around the outer periphery of the shielding layer 150 .

[0112] In this manner, the power cable 10 is manufactured as a solid insulated power cable.

[0113] (5) Summary of this embodiment According to this embodiment, one or more of the following advantages are achieved.

[0114] (a) The resin composition of this embodiment has a viscosity of 200 Pa·s to 5000 Pa·s at a high shear rate. This allows the resin composition to be stably extruded with a uniform thickness while maintaining the extrusion shape when melted and extruded. In addition, the viscosity of this resin composition at a low shear rate is 7000 Pa·s to 50000 Pa·s. This allows the extruded resin composition to be cooled and its shape fixed, preventing sagging due to its own weight, and making it easy to maintain the extrusion shape. Thus, the resin composition of this embodiment has excellent extrusion moldability, but is not easily flowable in a molten state and is not easily deformed.

[0115] (b) According to the resin composition of the present embodiment, when the insulating layer 130 of the power cable 10 is formed, the insulating layer 130 can be formed to a uniform thickness in both the circumferential direction of the cross section and the longitudinal direction of the power cable 10. As a result, the variation in the outer diameter of the power cable 10 can be reduced in the cross section and the longitudinal direction. Specifically, in the cross section of the power cable 10, the ratio of the maximum outer diameter (major axis) to the minimum outer diameter (minor axis) in the circumferential direction can be set to 1.3 or less. Furthermore, in two cross sections spaced apart in the longitudinal direction of the power cable 10, the ratio of the major axis at one point to the minor axis at the other point can be set to 1.3 or less.

[0116] (c) Furthermore, the resin composition of the present embodiment is configured to have an elastic modulus of 150 MPa or more and 700 MPa or less. Therefore, in the insulating layer 130, the AC breakdown field strength can be kept high, and a predetermined insulating property can be ensured. Specifically, the AC breakdown field strength can be made 60 kV / mm or more.

[0117] (d) By including at least one of a rubber material and an elastomer in addition to the propylene-based resin, excessive crystal growth of the propylene-based resin can be suppressed during the process of cooling from a molten state, thereby enabling the insulating layer 130 to achieve a high level of insulation and flexibility in a well-balanced manner.

[0118] (e) The melting point of the resin composition may be 140°C to 150°C if it contains random PP, and 158°C to 168°C if it contains homo PP. The heat of fusion may be 60J / g to 100J / g if it contains random PP, and 75J / g to 110J / g if it contains homo PP. In the resin composition, by satisfying at least one of the melting point and heat of fusion within a predetermined range, the addition ratio of the propylene-based resin, the rubber material, and the elastomer can be set within an appropriate range, and the viscosity at high shear rate and low shear rate can be reliably adjusted within the above range. Moreover, the insulating layer 130 can obtain a high level of insulation and flexibility in a well-balanced manner.

[0119] (f) Furthermore, according to the resin composition, even when the thickness of the insulating layer 130 is 4 mm or more and the ratio of the outer diameter of the power cable 10 to the outer diameter of the conductor 110 is 4 or less, that is, even when the insulating layer 130 is formed to be thicker than the outer diameter of the conductor 110, the fluctuation in the outer diameter can be kept small.

[0120] (g) Furthermore, by using the resin composition, during production of the power cable 10, it is possible to suppress fluctuations in outer diameter in the longitudinal direction, which is particularly likely to occur when a vertical extruder is used, and fluctuations in outer diameter in the circumferential direction of the cross section, which is particularly likely to occur when a horizontal extruder is used.

[0121] (h) Furthermore, by using the resin composition, the ratio of the major axis to the minor axis in the cross section of the power cable 10 can be made small, for example, 1.3 or less, so that the uniformity of the outer diameter can be increased, thereby shortening the processing time when connecting the power cable 10. Furthermore, when the power cable 10 is connected to a connecting member, voids at the connection point can be suppressed, and the connection can be made more reliably.

[0122] <Other embodiments of the present disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above-described embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.

[0123] In the above-described embodiment, the resin composition molded body as the insulating layer is described as being one which is mechanically mixed and extrusion molded, but the resin composition molded body may also be one which is polymerized and extrusion molded.

[0124] In the above embodiment, the case where the power cable 10 does not need to have a water-shielding layer has been described, but the present disclosure is not limited to this case. The power cable 10 may have a simple water-shielding layer because it has the above-mentioned remarkable water tree suppression effect. Specifically, the simple water-shielding layer is made of, for example, a metal laminate tape. The metal laminate tape has, for example, a metal layer made of aluminum or copper, and an adhesive layer provided on one or both sides of the metal layer. The metal laminate tape is, for example, wound by longitudinal splicing so as to surround the outer periphery of the cable core (outer periphery than the outer semiconductive layer). The water-shielding layer may be provided outside the shielding layer, or may also serve as the shielding layer. With such a configuration, the cost of the power cable 10 can be reduced.

[0125] In the above embodiment, the power cable 10 is configured to be laid on land, underwater, or on the bottom of the water, but the present disclosure is not limited to this. For example, the power cable 10 may be configured as a so-called overhead electric wire (overhead insulated electric wire).

[0126] In the above embodiment, three layers are simultaneously extruded in the cable core forming step S300, but each layer may be extruded one at a time. EXAMPLES

[0127] Next, examples according to the present disclosure will be described. These examples are merely examples of the present disclosure, and the present disclosure is not limited to these examples.

[0128] (1) Material As resin compositions for forming an insulating layer, materials A to E shown in the following Table 1 were prepared. In preparing materials A to E, the following components were used.

[0129] As the propylene-based resin, multiple types of propylene random polymers different from each other were prepared, each having a viscosity at a high shear rate of 100 Pa·s or more and 6000 Pa·s or less, a viscosity at a low shear rate of 500 Pa·s or more and 50,000 Pa·s or less, a melting point of 140°C or more and 145°C or less, a heat of fusion of 90 J / g or more and 105 J / g or less, an elastic modulus of 600 MPa or more and 1200 MPa or less, a ratio Mw / Mn of weight average molecular weight (Mw) to number average molecular weight (Mn) of 3.0 or more and 8.0 or less, and Mn in the range of 60,000 to 150,000 and Mw in the range of 210,000 to 1,000,000.

[0130] The rubber materials prepared were several different types of EPR and VLDPE, with different viscosities at high shear rate of 500 Pa·s to 5000 Pa·s, and at low shear rate of 10,000 Pa·s to 70,000 Pa·s, no melting point or heat of fusion, elastic modulus of 1 MPa to 200 MPa, Mw / Mn of 1.0 to 3.0, Mn of 70,000 to 250,000, and Mw of 70,000 to 600,000.

[0131] As the elastomers, multiple types of styrene-based resins were prepared that were different from one another in terms of viscosity at high shear rate within the ranges of 1000 Pa·s to 6000 Pa·s, viscosity at low shear rate within the ranges of 5000 Pa·s to 50,000 Pa·s, melting point within the ranges of 30°C to 80°C, heat of fusion within the ranges of 5 J / g to 50 J / g, elastic modulus within the ranges of 1 MPa to 200 MPa, Mw / Mn within the ranges of 1.0 to 3.0, Mn within the ranges of 70,000 to 250,000, and Mw within the ranges of 70,000 to 600,000.

[0132] In this example, one or more propylene-based resins having physical properties within the above ranges were used alone or in combination, and one or more rubber materials or elastomers having physical properties within the above ranges were used. The ratio of each component was appropriately changed so that the viscosity of the resulting resin composition was a predetermined value, and materials A to E shown in Table 1 were prepared. Here, the addition ratio of the propylene-based resin was adjusted to 50% by mass or more of the resin composition. Material E was prepared by further adding 5 parts by mass of inorganic filler to 100 parts by mass of the resin component.

[0133] [Table 1]

[0134] In addition, the melting point, heat of fusion, viscosity at high shear rate, viscosity at low shear rate, and elastic modulus of each of the materials A to E in Table 1 were measured as follows.

[0135] (Melting point and heat of fusion) The melting points and heat of fusion of materials A to E were determined by DSC measurement. The DSC measurement was performed in accordance with JIS-K-7121 (1987). Specifically, a PerkinElmer DSC8500 (input compensation type) was used as the DSC device. The reference sample was, for example, α-alumina. The mass of the measurement sample was 8 to 10 g. In the DSC device, the temperature was raised from room temperature (27°C) to 220°C at a rate of 10°C / min. Thus, the amount of heat absorbed (heat flow) per unit time was plotted against the temperature to obtain a DSC curve.

[0136] The temperature at which the amount of heat absorbed per unit time in each sample reached its maximum (highest peak) was taken as the "melting point." The area of ​​the region enclosed by the melting peak and the baseline in the DSC curve was calculated to determine the "heat of fusion."

[0137] (viscosity) The viscosity of materials A to E at each shear rate was measured using a rotational rheometer (Anton Paar's "MCR302") at 190 °C and a shear rate of 0.001 s -1 From 1000s -1 The shear rate was changed up to 1000 s.

[0138] (Elasticity Modulus) The elastic modulus of materials A to E was measured by dynamic mechanical analysis (DMA). Specifically, first, a press sheet for evaluation was prepared from each material. The press sheet was subjected to 0.08% expansion and contraction, and the storage elastic modulus of the press sheet was measured while heating it from -50°C to 100°C. The measurement frequency was 10Hz. The heating rate was 10°C / min. As a result of the measurement, the storage elastic modulus at 25°C was obtained.

[0139] (2) Preparation of a sample power cable In this example, materials A to E were used as resin compositions for forming an insulating layer to produce a sample simulating a power cable.

[0140] (Sample 1) Specifically, as shown in Table 2 below, first, the cross-sectional area is 2500 mm 2A conductor (conductor diameter: about 56.4 mm) was prepared. After the conductor was prepared, the resin composition for the internal semiconductive layer containing an ethylene-ethyl acrylate copolymer, the above-mentioned material A as a resin composition for forming an insulating layer, and the resin composition for the external semiconductive layer made of the same material as the resin composition for the internal semiconductive layer were respectively fed into extruders A to C. The extrudates from extruders A to C were guided to a common head, and the internal semiconductive layer, the insulating layer, and the external semiconductive layer were simultaneously extruded from the inside to the outside around the conductor. At this time, the thicknesses of the internal semiconductive layer, the insulating layer, and the external semiconductive layer were 1.0 mm, 24 mm, and 1.0 mm, respectively, and the insulating coating thickness was 26 mm. As a result, a power cable sample 1 (cable outer diameter: 108.4 mm) having a conductor, an internal semiconductive layer, an insulating layer, and an external semiconductive layer from the center to the periphery was produced. In addition, when the conductor diameter is X and the outer diameter of the power cable (outer cable diameter) is Y, the ratio of the outer cable diameter to the conductor diameter (Y / X) is 1.9.

[0141] In addition, the resin composition for forming the insulating layer was changed from material A to material B, and a power cable was produced with the same cable configuration.

[0142] (Samples 2-11) For Samples 2 to 11, as shown in Table 2 below, Material A or Material B was used as the resin composition for forming the insulating layer, and the conductor diameter and the insulating coating thickness were changed, but other than that, power cables were produced in the same manner as for Sample 1 to obtain Samples 2 to 11. Note that, in each sample, the thicknesses of the inner semiconductive layer and the outer semiconductive layer were the same, and the insulating coating thickness was appropriately changed by adjusting the thickness of the insulating layer.

[0143] [Table 2]

[0144] (Samples 12-14) In addition, for samples 12 to 14, materials C to E were used as the resin compositions for forming the insulating layer, as shown in Table 3 below, and power cables were produced in the same manner as sample 1, except that the conductor diameter and insulating coating thickness were appropriately changed.

[0145] [Table 3]

[0146] (3) Evaluation For Samples 1 to 14 produced as power cables, the uniformity of the outer diameter in the cross section of the power cable, the uniformity of the outer diameter in the longitudinal direction, and the insulation properties were evaluated.

[0147] The uniformity of the outer diameter in the cross section was evaluated as follows. Specifically, an arbitrary point in the longitudinal direction of the power cable was selected, and the outer diameter in the circumferential direction in the cross section was measured, the major axis (maximum value) and the minor axis (minimum value) were obtained, and the ratio of the major axis to the minor axis was calculated. The smaller this ratio, the smaller the variation in the outer diameter in the cross section.

[0148] The uniformity of the outer diameter in the longitudinal direction was evaluated as follows. Specifically, two points 5 m apart in the longitudinal direction of the power cable were selected, the long and short diameters were measured at each point, and the ratio of the long diameter at one point to the short diameter at the other point was calculated. The smaller this ratio, the smaller the variation in the outer diameter in the longitudinal direction.

[0149] The insulation was evaluated by an AC breakdown test. Specifically, a measurement sample was cut out to a thickness of 0.2 mm from the insulating layer of the prepared sample. Then, at room temperature (27°C), an AC voltage of commercial frequency (e.g., 60 Hz) was applied to the 0.2 mm thick measurement sample at 10 kV for 10 minutes, and then increased in 1 kV increments for 10 minutes, and this was repeated. The electric field strength was measured when the inner sample experienced insulation breakdown. As a result, an AC breakdown strength of 60 kV / mm or more was evaluated as good.

[0150] (4) Evaluation results The evaluation results are summarized in Tables 2 and 3.

[0151] As shown in Table 2, it was confirmed that in Samples 1 to 11, when Material A was used as the resin composition for forming the insulating layer, the fluctuation in the outer diameter in both the cross section and the longitudinal direction tended to be smaller than when Material B was used. This is because Material B is more likely to sag than Material A and is unable to maintain its shape.

[0152] Specifically, as shown in Table 1, it was confirmed that the viscosity of material B at high shear rate was 1000 Pa·s, which was in the range of 200 Pa·s to 5000 Pa·s, and therefore the resin composition could be stably extruded with a constant thickness. On the other hand, since the viscosity at low shear rate was 5000 Pa·s, which was less than 7000 Pa·s, material B was prone to flow and sag after extrusion until the shape was fixed by cooling. Therefore, it is presumed that when material B was used, the insulating layer deformed before the shape was fixed, and the outer diameter of the power cable changed accordingly. With material B, if the insulating coating thickness was small or the ratio (Y / X) of the cable outer diameter to the conductor diameter X was small, as shown in samples 2 and 8, the outer diameter fluctuation could be suppressed, but it was confirmed that if the insulating coating thickness was 4 mm or more or Y / X was large, the outer diameter fluctuation became larger, as shown in samples 1, 3 to 7, and 9 to 11.

[0153] In contrast, material A has a low viscosity at high shear rates and is excellent in extrusion moldability, but also has a high viscosity at low shear rates and is less likely to flow in a molten state than material B. Therefore, material A can suppress outer diameter fluctuations compared to material B.

[0154] Also, as shown in Samples 2, 8, and 9, it was confirmed that when the thickness of the insulating coating was reduced, the outer diameter fluctuation was unlikely to occur. As shown in Samples 7, 10, and 11, it was confirmed that when a power cable was manufactured so that the ratio of the cable outer diameter to the conductor diameter was excessively high, the outer diameter fluctuation was likely to occur. Furthermore, as shown in Samples 1, 3 to 6, it was confirmed that, according to Material A, if the thickness of the insulating layer was set to 4 mm or more and the ratio of the cable outer diameter to the conductor diameter was set to 4 or less, the outer diameter fluctuation could be suppressed to a ratio of 1.3 or less.

[0155] Also, as shown in Sample 12, it was confirmed that Material C had poor extrusion moldability due to excessively high viscosity at high shear rates, and could not be molded into an insulating layer. On the other hand, as shown in Sample 13, it was confirmed that Material D had too low viscosity at both high and low shear rates, and therefore could not be extruded in a stable shape, and could not maintain the extruded shape, and therefore could not be molded into an insulating layer.

[0156] In addition, as shown in Sample 14, since Material E contains an inorganic filler, the viscosity at both high shear rates and low shear rates is large, and therefore, it was confirmed that the extrudability of the resin composition is unstable, and the outer diameter fluctuation, particularly in the longitudinal direction, is large.

[0157] In addition, it was confirmed that, among samples 1 to 14, when the uniformity of the outer diameter in the cross-section and longitudinal direction was high and the ratio of outer diameter fluctuation was 1.3 or less, the AC breakdown strength was 60 kV / mm or more, and high insulation properties could be obtained more reliably.

[0158] <Additional Notes> The following additional aspects of the present disclosure.

[0159] (Appendix 1) A propylene-based resin, at least one of a rubber material and an elastomer; The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; Temperature: 190℃, shear rate: 100s -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less, The elastic modulus is 150 MPa or more and 700 MPa or less. Resin composition.

[0160] (Appendix 2) A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; The resin composition comprises A propylene-based resin, at least one of a rubber material and an elastomer; The rubber materials and elastomers have at least two units of ethylene, propylene, butylene, hexene, isoprene, octene, and styrene; The temperature of the resin composition was 190°C and the shear rate was 100 s -1 Viscosity at high shear rate is 200 Pa s or more and 5000 Pa s or less, temperature is 190°C, shear rate is 1 s -1 The viscosity at low shear rate is 7000 Pa s or more and 50000 Pa s or less, The elastic modulus is 150 MPa or more and 700 MPa or less. Power cable.

[0161] (Appendix 3) The heat of fusion of the resin composition is 60 J / g or more and 100 J / g or less. 2. A power cable as defined in claim 2.

[0162] (Appendix 4) The melting point of the resin composition is 140°C or higher and 150°C or lower. 4. The power cable according to claim 2 or 3.

[0163] (Appendix 5) In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less. 5. The power cable according to claim 2,

[0164] (Appendix 6) In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less. 6. The power cable according to claim 2,

[0165] (Appendix 7) The thickness of the insulating layer is 4 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less. 7. The power cable according to claim 2,

[0166] (Appendix 8) The propylene-based resin has an elastic modulus of 600 MPa or more and 1200 MPa or less. 8. The power cable according to claim 2,

[0167] (Appendix 9) The propylene-based resin has a viscosity of 100 Pa·s or more and 6000 Pa·s or less at the high shear rate and a viscosity of 500 Pa·s to 50000 Pa·s or less at the low shear rate. 10. The power cable according to claim 2,

[0168] (Appendix 10) The propylene-based resin has a melting point of 140° C. or more and 150° C. or less and a heat of fusion of 90 J / g or more and 105 J / g or less. 10. The power cable according to any one of appendixes 2 to 9.

[0169] (Appendix 11) The propylene-based resin has a ratio Mw / Mn of 3.0 or more and 8.0 or less, where Mw is the weight average molecular weight and Mn is the number average molecular weight in the molecular weight distribution. 11. The power cable according to claim 2.

[0170] (Appendix 12) The rubber material and the elastomer have a viscosity of 300 Pa·s or more and 7000 Pa·s or less at the high shear rate and a viscosity of 4000 Pa·s or more and 80000 Pa·s or less at the low shear rate. Attachment 2. A power cable according to claim 1.

[0171] (Appendix 13) The rubber material and the elastomer have an elastic modulus of 1 MPa or more and 200 MPa or less. Attachment 2. A power cable according to any one of claims 2 to 12.

[0172] (Appendix 14) The rubber material has no melting point or has a melting point of 100°C or less. Attachment 2 to 13. A power cable according to any one of claims 2 to 13.

[0173] (Appendix 15) The rubber material has a heat of fusion of 50 J / g or less. Attachment 2. A power cable according to claim 1.

[0174] (Appendix 16) In the rubber material and the elastomer, when the weight average molecular weight in the molecular weight distribution is Mw and the number average molecular weight is Mn, the ratio Mw / Mn is 1.0 or more and 3.0 or less. Attachment 2 to 15. A power cable according to any one of claims 2 to 15. [Explanation of symbols]

[0175] 10 Power Cable 110 Conductor 120 Inner semiconducting layer 130 Insulating layer 140 Outer semiconducting layer 150 Shielding layer 160 Sheath

Claims

1. A conductor; an insulating layer formed from a resin composition and covering the outer periphery of the conductor; The resin composition comprises The composition includes a mixture of a propylene-based resin, a rubber material, and an elastomer, The propylene-based resin is at least one of a propylene homopolymer having a melting point of 160° C. or more and 175° C. or less and a propylene random polymer having a melting point of 140° C. or more and 150° C. or less, The rubber material is a copolymer of at least two of ethylene, propylene, butene, hexene, and octene, has no melting point, the elastomer is a styrene-based thermoplastic elastomer containing styrene as a hard segment and at least one of ethylene, propylene, butene, and isoprene as a soft segment, and has no melting point or a melting point of 100° C. or lower; Temperature: 190°C, shear rate: 100s -1 The viscosity at high shear rate is 200 Pa·s or more and 5000 Pa·s or less, at a temperature of 190°C and a shear rate of 1 s -1 The viscosity at a low shear rate is 7000 Pa s or more and 50000 Pa s or less, The melting point of the resin composition is 158° C. or more and 168° C. or less when the propylene-based resin is the propylene homopolymer, and is 140° C. or more and 150° C. or less when the propylene-based resin is the propylene random polymer, The elastic modulus is 150 MPa or more and 700 MPa or less. Power cable.

2. The heat of fusion of the resin composition is 60 J / g or more and 100 J / g or less.

2. The power cable according to claim 1.

3. The propylene-based resin has a viscosity of 100 Pa·s or more and 6000 Pa·s or less at the high shear rate and a viscosity of 500 Pa·s or more and 50000 Pa·s or less at the low shear rate.

3. The power cable according to claim 1 or 2.

4. The rubber material and the elastomer have a viscosity at the high shear rate of 300 Pa·s or more and 7000 Pa·s or less, and a viscosity at the low shear rate of 4000 Pa·s or more and 80000 Pa·s or less.

3. The power cable according to claim 1 or 2.

5. In a cross section perpendicular to the longitudinal direction, the ratio of the major axis to the minor axis is 1.3 or less.

3. The power cable according to claim 1 or 2.

6. In a cross section taken at two points spaced apart in the longitudinal direction, the ratio of the major axis at one point to the minor axis at the other point is 1.3 or less.

3. The power cable according to claim 1 or 2.

7. The thickness of the insulating layer is 4 mm or more, and the ratio of the outer diameter of the power cable to the outer diameter of the conductor is 4 or less.

3. The power cable according to claim 1 or 2.

8. The propylene-based resin accounts for 50% by mass or more of the resin composition.

3. The power cable according to claim 1 or 2.

Citation Information

Patent Citations

  • Insulating compositon for power cable

    JP1982069611A

  • High-modulus, impact-resistant polyolelfin resin composition

    JP1987179545A

  • Low-smoke self-extinguishing cable and flame-retardant composition used therefor

    JP2001511582A

  • Polyolefin compound for cable coating

    JP2018514051A

  • Polypropylene resin for insulator of power cable

    JP2019073678A