Method for manufacturing a medical device
A method using (co)polymer of (meth)acrylamide with specific properties in an aqueous packaging liquid at controlled pH and concentration enhances the durability and hydrophilicity of medical devices, addressing the limitations of existing surface modification techniques.
Patent Information
- Application Number
- JP2020527983
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-20
- Filing Date
- 2020-04-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-04-16
AI Technical Summary
Existing methods for surface modification of medical devices, such as contact lenses, fail to provide sufficient durability and hydrophilicity, often requiring additional washing and sterilization steps, and struggle with controlling the number of acid terminals in polymer treatments.
A method involving heating a medical device in an aqueous packaging liquid containing a (co)polymer of (meth)acrylamide with two substituents having 2 or more carbon atoms on the nitrogen atom, at a concentration of 0.0001 to 30 mass % and a pH of 6.1 to 8.0, which can be used as a sterilization step, ensuring excellent durability and hydrophilicity.
The method achieves medical devices with enhanced durability and hydrophilicity without additional manufacturing steps, maintaining water wettability and slipperiness, applicable to various medical devices including contact lenses and other ophthalmic lenses, skin dressings, and biosensor chips.
Smart Images

Figure 0007585786000001 
Figure 0007585786000002 
Figure 0007585786000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a medical device. [Background technology]
[0002] 2. Description of the Related Art Conventionally, devices using soft resin materials such as silicone rubber and hydrogels, and devices using hard materials such as metals and glass have been used for a variety of purposes in various fields.
[0003] Applications of devices using soft materials include medical devices that are introduced into the body or that cover the surface of the body, biotechnology devices such as cell culture sheets and scaffolding materials for tissue regeneration, and cosmetic devices such as facial packs.
[0004] Applications of devices using hard materials include electrical appliances such as personal computers, mobile phones, and displays, as well as diagnostic and analytical tools such as ampoules for injectable drugs, capillary tubes, and biosensing chips.
[0005] When various devices are used, for example, as medical devices by being introduced into a living body or attached to the surface of a living body, it is important to modify the surface of the substrate of the medical device in order to improve its biocompatibility. If the surface modification can give the medical device better properties than before the surface modification, such as hydrophilicity, slipperiness, biocompatibility, and medicinal properties, users (patients, etc.) can expect improved usability, reduced discomfort, and improved symptoms.
[0006] Various methods are known for modifying the surface of the substrate of a medical device.
[0007] For example, Patent Document 1 discloses a method for imparting good water wettability to the surface of a substrate by heating the substrate in a solution containing a polymer having a hydroxyl group and having a pH of 2.0 or more and 6.0 or less.
[0008] Also known is a method for improving the wearability of a substrate by autoclaving the substrate in a solution containing one or more polymer materials and having a pH in the range of 6 to 9 (see, for example, Patent Documents 2 to 4). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2017 / 146102 [Patent Document 2] Special Publication No. 2011-512546 [Patent Document 3] Special Publication No. 2003-535626 [Patent Document 4] Patent No. 5154231 Summary of the Invention [Problem to be solved by the invention]
[0010] However, in the surface modification method of the substrate as described in Patent Document 1, the pH of the solution containing the substrate after heating is 6.0 or less. Therefore, when used in medical devices such as ophthalmic lenses, it is necessary to perform additional washing and sterilization steps in a neutral solution to prevent irritation to the eyes. This may lead to an increase in manufacturing costs.
[0011] As described in Patent Document 2, for contact lenses in which the substrate is immersed in a packaging solution containing acid-terminated polyvinylpyrrolidone and sterilized by autoclave, there is no specific description of the durability of water wettability, and it is difficult to expect that the water wettability will be maintained with sufficient durability to withstand scrubbing. In addition, although acid-terminated polyvinylpyrrolidone is specifically prepared in the examples, the method involves reacting hydroxyl-functionalized poly(vinylpyrrolidone) and poly(vinylpyrrolidone-co-allyl alcohol), which are polymers, with succinic anhydride, and there is a problem in that it is difficult to control the number of acid termini introduced.
[0012] In the surface modification method of a substrate as described in Patent Document 3, specific surface treatments using poly(acrylic acid-co-acrylamide) and poly(acrylic acid-co-vinylpyrrolidone) were investigated, but the hydrophilicity and other properties of the substrate surface were insufficient.
[0013] In the surface modification method of the substrate as described in Patent Document 4, when the surface treatment was specifically conducted using polyvinylpyrrolidone, the hydrophilicity and other properties of the substrate surface were still insufficient.
[0014] The present invention has been made in consideration of the problems inherent in the conventional techniques described above. That is, an object of the present invention is to provide a method for easily producing a medical device having excellent durability and hydrophilicity. [Means for solving the problem]
[0015] In order to achieve the above object, the present invention A method for producing a medical device, comprising the step of heating an aqueous packaging solution, the heating being carried out in a state in which one or more hydrophilic polymers are contained in the aqueous packaging solution and at least a portion of a substrate of the medical device is in contact with the aqueous packaging solution; The present invention relates to a method for manufacturing a medical device, which satisfies all of the following requirements (a) to (c). (a) The hydrophilic polymer is a (co)polymer of (meth)acrylamide having two substituents having two or more carbon atoms on the nitrogen atom. (b) the mass % concentration of the hydrophilic polymer contained in the aqueous packaging liquid is in the range of 0.0001 to 30 mass %; (c) The pH of the aqueous packaging solution after the heating step is in the range of 6.1 to 8.0. Effect of the Invention
[0016] According to the present invention, unlike the prior art, a medical device having excellent durability and imparted hydrophilicity can be easily obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The method for producing a medical device of the present invention is a method for producing a medical device, comprising the step of heating an aqueous packaging liquid, the heating step being carried out in a state in which one or more types of hydrophilic polymers are contained in the aqueous packaging liquid and at least a portion of a substrate of the medical device is in contact with the aqueous packaging liquid; The present invention relates to a method for manufacturing a medical device, which satisfies all of the following requirements (a) to (c). (a) The hydrophilic polymer is a (co)polymer of (meth)acrylamide having two substituents having two or more carbon atoms on the nitrogen atom. (b) the mass % concentration of the hydrophilic polymer contained in the aqueous packaging liquid is in the range of 0.0001 to 30 mass %; (c) The pH of the aqueous packaging solution after the heating step is in the range of 6.1 to 8.0. In the present invention, "(meth)acrylamide having two substituents having two or more carbon atoms on the nitrogen atom" means that the nitrogen atom of the (meth)acrylamide has two substituents having two or more carbon atoms other than the (meth)acryl group.
[0018] In the present invention, "(meth)acrylamide" includes both acrylamide and methacrylamide. The same applies to "(meth)acrylate" and "(meth)acrylic acid." Furthermore, "(co)polymer" includes both homopolymers and copolymers.
[0019] In the present invention, the medical device may have a lens shape, and is preferably an ophthalmic lens. Examples of medical devices having a lens shape include ophthalmic lenses such as contact lenses, intraocular lenses, artificial corneas, corneal inlays, corneal onlays, and eyeglass lenses. Ophthalmic lenses, and among them, contact lenses, are one of the most preferred embodiments of the present invention.
[0020] In the present invention, the medical device may be in the form of a tube. Examples of tubular medical devices include infusion tubes, gas transport tubes, drainage tubes, blood circuits, covering tubes, catheters, stents, sheaths, tube connectors, access ports, and hollow fibers for cardiopulmonary bypass.
[0021] In the present invention, the medical device may be in the form of a sheet or film. Examples of the medical device in the form of a sheet or film include a skin dressing, a wound dressing, a skin protection material, a drug carrier for skin, a biosensor chip, and a dressing for an endoscope.
[0022] In the present invention, the medical device may have a container shape. Examples of the medical device having a container shape include a drug carrier, a cuff, and a drainage bag.
[0023] In the present invention, the medical device is preferably an ophthalmic lens, a skin covering material, a wound covering material, a skin protective material, a skin drug carrier, a transfusion tube, a gas transport tube, a drainage tube, a blood circuit, a covering tube, a catheter, a stent, a sheath biosensor chip, an artificial heart-lung machine, or a covering material for an endoscope. The medical device is more preferably an ophthalmic lens.
[0024] In particular, in one of the most preferred embodiments of the present invention, the ophthalmic lens is a contact lens. In the present invention, the contact lens includes both contact lenses for vision correction and cosmetic purposes.
[0025] In the present invention, the substrate of the medical device can be either a hydrous substrate or a non-hydrous substrate. Examples of the material of the hydrous substrate include hydrogel and silicone hydrogel. Silicone hydrogel is particularly preferred because it has flexibility and high oxygen permeability that provides an excellent wearing sensation. Examples of the material of the non-hydrous substrate include low hydrous soft material and low hydrous hard material. That is, in the manufacturing method of the medical device of the present invention, it is preferable that the substrate includes one or more materials selected from the group consisting of hydrogel, silicone hydrogel, low hydrous soft material, and low hydrous hard material.
[0026] The present invention is applicable to both general hydrogels not containing silicone and hydrogels containing silicone (i.e., silicone hydrogels) as the material of the water-absorbent substrate. The present invention is particularly suitable for silicone hydrogels because it can greatly improve the surface properties.
[0027] Hereinafter, United States Adopted Names (USAN) may be used to represent materials. In USAN, a symbol such as A, B, or C may be added to the end of the name to represent a material variant, but in this specification, when no symbol is added to the end, all variants are represented. For example, simply writing "ocufilcon" represents all variants of ocufilcon, such as "ocufilconA", "ocufilconB", "ocufilconC", "ocufilconD", "ocufilconE", and "ocufilconF".
[0028] In the method for producing a medical device of the present invention, the hydrogel is preferably a hydrogel selected from the group consisting of tefilcon, tetrafilcon, helfilcon, mafilcon, polymacon, hioxifilcon, alfafilcon, omafilcon, nelfilcon, nesofilcon, hilafilcon, acofilcon, deltafilcon, etafilcon, focofilcon, ocufilcon, phemfilcon, methafilcon, and vilfilcon.
[0029] For example, when the hydrogel is a contact lens, it is classified into Group 1 to Group 4 according to the contact lens classification defined by the U.S. Food and Drug Administration (FDA). Among them, Group 2 and Group 4 are more preferable, and Group 4 is particularly preferable, since they exhibit good water wettability and antifouling properties.
[0030] Group 1 refers to non-ionic hydrogel lenses with a water content of less than 50% by mass, specifically including tefilcon, tetrafilcon, helfilcon, mafilcon, polymacon, and hioxifilcon.
[0031] Group 2 refers to non-ionic hydrogel lenses with a water content of 50% by mass or more. Specific examples include alfafilcon, omafilcon, hioxifilcon, nelfilcon, nesofilcon, hilafilcon, and acofilcon. Because of their excellent water wettability and antifouling properties, omafilcon, hioxifilcon, nelfilcon, and nesofilcon are more preferred, omafilcon and hioxifilcon are even more preferred, and omafilcon is particularly preferred.
[0032] Group 3 refers to ionic hydrogel lenses with a water content of less than 50% by mass, specifically, deltafilcon.
[0033] Group 4 refers to ionic hydrogel lenses with a water content of 50% by mass or more. Specific examples include etafilcon, focofilcon, ocufilcon, pemfilcon, methafilcon, and vilfilcon. Since they exhibit good water wettability and antifouling properties, etafilcon, focofilcon, ocufilcon, and pemfilcon are more preferred, etafilcon and ocufilcon are even more preferred, and etafilcon is particularly preferred.
[0034] As a specific example of the silicone hydrogel, when the silicone hydrogel is a contact lens, a silicone hydrogel selected from the group belonging to Group 5 of the contact lens classification defined by the US Food and Drug Administration (FDA) is preferable.
[0035] The silicone hydrogel is preferably a polymer that contains silicon atoms in the main chain and / or side chain and has hydrophilic properties, and examples thereof include copolymers of a monomer containing a siloxane bond and a hydrophilic monomer.
[0036] Specifically, the silicone hydrogel is preferably selected from the group consisting of lotrafilcon, galyfilcon, narafilcon, senofilcon, comfilcon, enfilcon, balafilcon, efrofilcon, fanfilcon, somofilcon, samfilcon, olifilcon, asmofilcon, formofilcon, stenfilcon, abafilcon, mangofilcon, riofilcon, sifilcon, larafilcon and delefilcon. Among them, because they show good water wettability and easy slipping, lotrafilcon, galyfilcon, narafilcon, senofilcon, comfilcon, enfilcon, stenfilcon, somofilcon, delefilcon, balafilcon and samfilcon are more preferred, lotrafilcon, narafilcon, senofilcon, comfilcon and enfilcon are even more preferred, and narafilcon, senofilcon and comfilcon are particularly preferred.
[0037] As the low water content soft material and the low water content hard material, for example, when used in medical devices such as ophthalmic lenses, it is preferable to use a material containing a silicon atom, since such a material exhibits high oxygen permeability that enables sufficient oxygen to be supplied to the cornea.
[0038] As a specific example of the low water content hard material, when the low water content hard material is a contact lens, the low water content hard material is preferably selected from the group belonging to the classification of contact lenses defined by the US Food and Drug Administration (FDA).
[0039] As such a low water content hard material, a polymer containing silicon atoms in the main chain and / or side chain is preferred. For example, a polymer containing siloxane bonds can be mentioned. Among these polymers containing silicon atoms, those in which the silicon atoms are contained in the polymer through siloxane bonds are preferred from the viewpoint of oxygen permeability. Specific examples of such polymers include homopolymers using tris(trimethylsiloxy)silylpropyl methacrylate, polydimethylsiloxane having double bonds at both ends, silicone-containing (meth)acrylate, etc., or copolymers of these monomers with other monomers.
[0040] Specifically, the low water content hard material is preferably a material selected from the group consisting of neofocon, pasifocon, telefocon, silafocon, paflufocon, petrafocon and fluorofocon. Among them, neofocon, pasifocon, telefocon and silafocon are more preferable, neofocon, pasifocon and telefocon are further preferable, and neofocon is particularly preferable, because they show good water wettability and antifouling properties.
[0041] In the present invention, when the medical device is in a form other than a contact lens, suitable examples of the low water content hard material include polyethylene, polypropylene, polysulfone, polyetherimide, polystyrene, polymethyl methacrylate, polyamide, polyester, epoxy resin, polyurethane, polyvinyl chloride, etc. Among them, since they exhibit good water wettability and antifouling properties, it is more preferable that the low water content hard material is polysulfone, polystyrene, polymethyl methacrylate, or polyamide, and particularly preferable that the low water content hard material is polymethyl methacrylate.
[0042] Specific examples of low water content soft materials include low water content soft materials used in medical devices having a water content of 10% by mass or less, an elastic modulus of 100 kPa to 2,000 kPa, and a tensile elongation of 50% to 3,000%, as described in WO 2013 / 024799. Elastofilcon is also suitable.
[0043] In the present invention, when the medical device is an embodiment other than an ophthalmic lens including a contact lens, suitable examples of the low water content soft material include silicone elastomer, soft polyurethane, polyvinyl acetate, ethylene-vinyl acetate copolymer, soft polyester resin, soft acrylic resin, soft polyvinyl chloride, natural rubber, various synthetic rubbers, etc.
[0044] According to the present invention, whether the substrate is hydrophilic or low hydrophilic, it is possible to impart appropriate hydrophilicity (water wettability) to the surface of the medical device. Therefore, the substrate may have a water content of 0 to 99% by mass. Since the effect of imparting appropriate hydrophilicity to the surface of the medical device is further enhanced, the substrate preferably has a water content of 0.0001% by mass or more, and particularly preferably has a water content of 0.001% by mass or more. The substrate preferably has a water content of 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.
[0045] When the medical device is a contact lens, the water content of the base material is preferably 15% by mass or more, and more preferably 20% by mass or more, since this makes it easier to ensure the movement of the lens inside the eye.
[0046] The hydrophilic polymer used in the method for producing the medical device of the present invention is usually a material different from that of the substrate, but may be the same material as that constituting the substrate as long as the desired effect is obtained.
[0047] The hydrophilic polymer is composed of a material having hydrophilicity. However, other additives may be included as long as they do not impair the expression of hydrophilicity. Here, the hydrophilic material is a material that is soluble in 100 parts by mass of water or a mixture of 100 parts by mass of water and 100 parts by mass of tert-butanol at room temperature (20 to 23°C) at 0.0001 parts by mass or more, more preferably soluble in 0.01 parts by mass or more, even more preferably soluble in 0.1 parts by mass or more, and particularly preferably soluble in 1 part by mass or more.
[0048] In the method for producing a medical device of the present invention, the (a) hydrophilic polymer is a (co)polymer of (meth)acrylamide having two substituents with 2 or more carbon atoms on the nitrogen atom. In the present invention, the (co)polymer of (meth)acrylamide having two substituents with 2 or more carbon atoms on the nitrogen atom means a (co)polymer containing (meth)acrylamide having two substituents with 2 or more carbon atoms on the nitrogen atom as a (co)polymerization component. Such a hydrophilic polymer is preferable because it can form a surface that is durable and has excellent water wettability.
[0049] The substituent having 2 or more carbon atoms may be linear or branched, and is preferably an alkyl group having 2 to 6 carbon atoms from the viewpoint of imparting good hydrophilicity to the medical device with good durability, such as an ethyl group, a 1-propyl group, a 2-propyl group, a 1-butyl group, a 2-butyl group, a tert-butyl group, a 1-pentyl group, a 2-pentyl group, a 3-pentyl group, and a hexyl group. In this specification, an alkyl group without a position number includes alkyl groups having all the position numbers of the alkyl group (for example, a "hexyl group" includes all of a "1-hexyl group", a "2-hexyl group", and the like). Among these, an ethyl group, a 1-propyl group, and a 2-propyl group are more preferable, and an ethyl group is particularly preferable.
[0050] As the combination of the two substituents in the above "having two substituents", a combination of the same substituents or a combination of different substituents can be suitably used. Specific examples of such (meth)acrylamides having two substituents with 2 or more carbon atoms on the nitrogen atom include N,N-diethyl(meth)acrylamide, N-ethyl-N-propyl(meth)acrylamide, and N-butyl-N-ethyl(meth)acrylamide. Among these, N,N-diethyl(meth)acrylamide is particularly preferred because it can impart good hydrophilicity to medical devices.
[0051] The above (meth)acrylamides can be used alone or in combination of two or more kinds.
[0052] In addition, the (co)polymer of (meth)acrylamide having two substituents having two or more carbon atoms on the nitrogen atom can also contain one or more types of other monomers having an amide group as a copolymerization component.
[0053] When a monomer having an amide group other than the above is contained as a copolymerization component, the hydrophilic polymer exhibits a suitable viscosity when dissolved in water, and thus a surface that is not only water wettable but also easily slippery can be formed. In the present invention, the amide group is a group containing a structure represented by NC=O.
[0054] As such other monomers having an amide group, from the viewpoint of ease of polymerization, monomers selected from monomers having a (meth)acrylamide group and N-vinyl carboxylic acid amides (including cyclic ones) are preferred.
[0055] Suitable examples of such monomers include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylacetamide, N-methyl-N-vinylacetamide, N-vinylformamide, N,N-dimethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-tert-butyl(meth)acrylamide, N-hydroxymethylacrylamide, N-methoxymethylacrylamide, and N-ethoxymethylacrylamide. Examples of the acrylic acid include N-vinylpyrrolidone, N-isopropyl(meth)acrylamide, N-(2-hydroxyethyl)(meth)acrylamide, N-butoxymethylacrylamide, N-isobutoxymethylacrylamide, N-hydroxymethylmethacrylamide, N-methoxymethylmethacrylamide, N-ethoxymethylmethacrylamide, N-propoxymethylmethacrylamide, N-butoxymethylmethacrylamide, N-isobutoxymethylmethacrylamide, acryloylmorpholine, and acrylamide. Among these, N-vinylpyrrolidone, N-isopropyl(meth)acrylamide, and N,N-dimethyl(meth)acrylamide are preferred in terms of lubricity, N-isopropyl(meth)acrylamide and N,N-dimethyl(meth)acrylamide are more preferred, and N,N-dimethyl(meth)acrylamide is particularly preferred.
[0056] When using a copolymer of (meth)acrylamide having two substituents with 2 or more carbon atoms on a nitrogen atom and a monomer having another amide group, the copolymerization ratio is preferably 1 / 99 to 99 / 1, where [mass of monomer having another amide group] / [mass of (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on a nitrogen atom]. The copolymerization ratio of the monomer having another amide group is more preferably 2% by mass or more, more preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more. The copolymerization ratio of the monomer having another amide group is more preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. The copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on a nitrogen atom is more preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. The copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on the nitrogen atom is more preferably 98% by mass or less, even more preferably 95% by mass or less, even more preferably 93% by mass or less, and even more preferably 90% by mass or less. If the copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on the nitrogen atom and the other monomer having an amide group is within the above range, functions such as water wettability and easy slipperiness are easily exhibited.
[0057] In the method for producing a medical device of the present invention, the hydrophilic polymer is preferably a copolymer of (meth)acrylamide having two substituents with two or more carbon atoms on the nitrogen atom and (meth)acrylic acid. Such a hydrophilic polymer is preferable because it can form a surface having excellent durability, excellent water wettability, and excellent antifouling properties against body fluids, etc.
[0058] Preferred specific examples of the copolymer of (meth)acrylamide and (meth)acrylic acid having two substituents with 2 or more carbon atoms on the nitrogen atom include a (meth)acrylic acid / N,N-diethylacrylamide copolymer, a (meth)acrylic acid / N-ethyl-N-propyl(meth)acrylamide copolymer, a (meth)acrylic acid / N-butyl-N-ethyl(meth)acrylamide copolymer, etc. Particularly preferred is a (meth)acrylic acid / N,N-diethyl(meth)acrylamide copolymer.
[0059] When using a copolymer of (meth)acrylamide having two substituents with 2 or more carbon atoms on a nitrogen atom and (meth)acrylic acid, the copolymerization ratio is preferably 1 / 99 to 99 / 1, i.e., [mass of (meth)acrylic acid monomer] / [mass of (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on a nitrogen atom]. The copolymerization ratio of the (meth)acrylic acid monomer is more preferably 2% by mass or more, even more preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more. The copolymerization ratio of the (meth)acrylic acid monomer is more preferably 90% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less, 60% by mass or less, 50% by mass or less, 40% by mass or less, and 30% by mass or less. The copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on the nitrogen atom is more preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, and 70% by mass or more. The copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on the nitrogen atom is more preferably 98% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and even more preferably 90% by mass or less. If the copolymerization ratio of the (meth)acrylamide monomer having two substituents with 2 or more carbon atoms on the nitrogen atom and the (meth)acrylic acid monomer is within the above range, functions such as water wettability and antifouling properties against body fluids are easily exhibited.
[0060] The (co)polymer of (meth)acrylamide having two substituents with two or more carbon atoms on the nitrogen atom may further contain one or more types of monomers other than (meth)acrylic acid that do not have an amide group as a copolymerization component. Hereinafter, the "monomer that does not have an amide group and is other than (meth)acrylic acid" may be referred to as monomer X.
[0061] Suitable examples of the monomer X include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, glycerol (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, N-(4-hydroxyphenyl)maleimide, hydroxystyrene, vinyl alcohol (with vinyl carboxylate as precursor). Among these, monomers having a (meth)acryloyl group are preferred in terms of ease of polymerization, and (meth)acrylic acid ester monomers are more preferred. From the viewpoint of improving antifouling properties against body fluids, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and glycerol (meth)acrylate are preferred, and hydroxyethyl (meth)acrylate is particularly preferred.
[0062] In addition, as the monomer X, it is also possible to use a monomer that exhibits functions such as hydrophilicity, antibacterial properties, antifouling properties, and medicinal properties.
[0063] Specific examples of antibacterial monomers include monomers having a quaternary ammonium salt, such as imidazolium salt monomers described in JP-A-2010-88858, (3-acrylamidopropyl)trimethylammonium chloride, trimethyl-2-methacryloyloxyethylammonium chloride, and 2-(meth)acryloyloxyethylphosphorylcholine.
[0064] When a (co)polymer of (meth)acrylamide having two substituents with 2 or more carbon atoms on a nitrogen atom contains a monomer X as a copolymerization component, the copolymerization ratio of the monomer X is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. The copolymerization ratio of the monomer X is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0065] When the copolymerization ratio of the (meth)acrylamide having two substituents having two or more carbon atoms on a nitrogen atom and the monomer X in the (co)polymer is within the above range, the (co)polymer is likely to exhibit functions such as water wettability, antifouling properties against body fluids, and antibacterial properties.
[0066] In addition, additives other than the above materials may be contained in the aqueous packaging solution as long as they do not impair the properties required for the medical device. Furthermore, in addition to the (co)polymer of (meth)acrylamide having two substituents with two or more carbon atoms on the nitrogen atom, one or more other hydrophilic polymers may be contained. However, since this increases the production cost, it is preferable that the hydrophilic polymer consists only of the (co)polymer of (meth)acrylamide having two substituents with two or more carbon atoms on one kind of nitrogen atom.
[0067] Here, one type of polymer means a polymer or a group of polymers (isomers, complexes, etc.) produced by one synthesis reaction. When a copolymer is produced using multiple monomers, polymers synthesized by varying the compounding ratio are not considered to be the same type, even if the constituent monomers are the same.
[0068] Furthermore, the hydrophilic polymer consisting of only a (co)polymer of (meth)acrylamide having two substituents with two or more carbon atoms on one kind of nitrogen atom means that the hydrophilic polymer does not contain any polymer other than the hydrophilic polymer, or even if it contains other polymers, the content of the other polymers is preferably 3 parts by mass or less per 100 parts by mass of the hydrophilic polymer. The content of the other polymers is more preferably 0.1 parts by mass or less, and even more preferably 0.0001 parts by mass or less.
[0069] When the other polymers contain basic groups, the ratio of the number of basic groups / acidic groups of all polymers contained in the aqueous packaging solution is preferably 0.20 or less. The ratio is more preferably 0.10 or less, and even more preferably 0.05 or less, since no salt is formed from the reaction between the acidic group and the basic group, and transparency is excellent. Here, the acidic group refers to an acidic functional group, and examples thereof include a group selected from a carboxyl group or a sulfonic acid group, and salts thereof. The basic group refers to a basic functional group, and examples thereof include an amino group and salts thereof.
[0070] Next, a method for producing the medical device of the present invention will be described. In the present invention, the medical device can be obtained by a method that includes a step of heating an aqueous packaging liquid, in which one or more kinds of hydrophilic polymers are contained in the aqueous packaging liquid, and the heating step is performed in a state in which at least a part of the substrate of the medical device is in contact with the aqueous packaging liquid, and that satisfies all of the specific requirements. Here, the inventors of the present invention have found that a medical device can be given hydrophilicity with excellent durability, that is, water wettability, which could not be achieved by conventional techniques, by a very simple method in which the hydrophilic polymer is a (co)polymer of (meth)acrylamide having two substituents with two or more carbon atoms on a nitrogen atom, and the aqueous packaging liquid has a mass % concentration of the hydrophilic polymer contained in the aqueous packaging liquid in the range of 0.0001 to 30 mass %, and at least a part of the medical device is heated in a state in which the medical device is in contact with the aqueous packaging liquid. In addition, the substrate that can be applied is not limited to a water-containing hydrogel and a silicone hydrogel. Furthermore, since the pH of the aqueous packaging solution after the heating step is 6.1 to 8.0, it is possible to impart excellent durability, water wettability, slipperiness, etc. to the medical device at the same time as the sterilization step, without increasing the manufacturing steps, particularly when the heating step is a sterilization step. This is of great industrial significance from the viewpoint of eliminating the need for additional manufacturing steps. Therefore, in the manufacturing method for the medical device of the present invention, it is preferable that the heating step is a sterilization step.
[0071] Next, the molecular weight and concentration of the hydrophilic polymer will be described. In the conventional technology, when the substrate surface is modified simultaneously with sterilization using only one type of hydrophilic polymer, it is difficult to impart sufficient water wettability and durable water wettability to the device. However, in the present invention, since the hydrophilic polymer has a high adsorption force to the substrate, even when the substrate surface is modified simultaneously with sterilization using only one type of hydrophilic polymer, it is easy to impart durable good water wettability and easy slipperiness to the substrate.
[0072] The hydrophilic polymer used in the present invention preferably has a molecular weight of 2,000 to 1,500,000. The molecular weight is more preferably 5,000 or more, and even more preferably 10,000 or more. The molecular weight is more preferably 1,200,000 or less, and even more preferably 1,000,000 or less. Here, the molecular weight is the weight average molecular weight in terms of polyethylene glycol measured by gel permeation chromatography (aqueous solvent).
[0073] In addition, regarding the concentration of the hydrophilic polymer in the aqueous packaging solution during production, if the concentration is too high, the viscosity may increase, which may make handling during production more difficult. Therefore, in the method for producing a medical device of the present invention, the mass % concentration of the hydrophilic polymer (b) is in the range of 0.0001 to 30 mass %. The concentration of the hydrophilic polymer is more preferably 0.001 mass % or more, and even more preferably 0.005 mass % or more. In addition, the concentration of the hydrophilic polymer is more preferably 10 mass % or less, even more preferably 5 mass % or less, more preferably 1 mass %, and most preferably 0.1 mass % or less.
[0074] In the heating step, since the medical device can be used as it is without adding a washing step after heating, (c) the pH of the aqueous packaging solution after the heating step is in the range of 6.1 to 8.0. The pH is more preferably 6.5 or more, more preferably 6.6 or more, even more preferably 6.7 or more, and even more preferably 6.8 or more. The pH is preferably 7.9 or less, more preferably 7.8 or less, and even more preferably 7.6 or less. If the pH is less than 6.1 or more than 8.0, when used in a medical device such as an ophthalmic lens, it is necessary to additionally perform a washing step and a sterilization step in a neutral solution to eliminate irritation to the eyes, which is not preferable since it complicates the manufacturing process.
[0075] The pH of the aqueous packaging solution may change slightly when the solution is heated, but the pH before the solution is also preferably in the range of 6.1 to 8.0 as described above.
[0076] The pH of the aqueous packaging solution can be measured using a pH meter (e.g., pH meter Eutech pH2700 (Eutech Instruments)). Here, the pH of the aqueous packaging solution before heating refers to the pH value measured after adding all of the hydrophilic polymer to the solution, stirring the solution at room temperature (20 to 23°C) for 30 minutes using a rotator, and homogenizing the solution. In the present invention, the pH value is rounded off to one decimal place.
[0077] As the solvent of the aqueous packaging solution containing the hydrophilic polymer, water-soluble organic solvent, water, and a mixed solvent thereof are preferred. A mixed solvent of water and a water-soluble organic solvent, and water are more preferred, and water is the most preferred. As the water-soluble organic solvent, various water-soluble alcohols are preferred, water-soluble alcohols having 6 or less carbon atoms are more preferred, and water-soluble alcohols having 5 or less carbon atoms are even more preferred. It is also preferable to further add a buffer to these solvents.
[0078] As the buffer, any known physiologically compatible buffer can be used. Buffers are known to those skilled in the art, and examples include the following: boric acid, borates (e.g., sodium borate), citric acid, citric acid salts (e.g., potassium citrate), bicarbonates (e.g., sodium bicarbonate), phosphate buffers (e.g., Na2HPO4, NaH2PO4, and KH2PO4), TRIS (tris(hydroxymethyl)aminomethane), 2-bis(2-hydroxyethyl)amino-2-(hydroxymethyl)-1,3-propanediol, bis-aminopolyols, triethanolamine, ACES (N-(2-acetamido)-2-aminoethanoyl esters), glycerol, ... sulfonic acid), BES (N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid), HEPES (4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid), MES (2-(N-morpholino)ethanesulfonic acid), MOPS (3-[N-morpholino]-propanesulfonic acid), PIPES (piperazine-N,N'-bis(2-ethanesulfonic acid)), TES (N-[tris(hydroxymethyl)methyl]-2-aminoethanesulfonic acid), and their salts.
[0079] The amount of each buffer is an amount necessary to effectively achieve a desired pH. Usually, the amount of the buffer in the solution is preferably 0.001% by mass to 2% by mass. The amount of the buffer is more preferably 0.01% by mass or more, and even more preferably 0.05% by mass or more. The amount of the buffer is more preferably 1% by mass or less, and even more preferably 0.30% by mass or less.
[0080] The pH of the buffer solution before containing the hydrophilic polymer is preferably 6.3 to 7.8, which is within the physiologically acceptable range. The pH of the buffer solution is preferably 6.5 or higher, more preferably 6.8 or higher. The pH of the buffer solution is preferably 7.6 or lower, more preferably 7.4 or lower.
[0081] The heating temperature is preferably 100° C. to 200° C., from the viewpoint of obtaining a medical device surface that has good water wettability and slipperiness and has little effect on the strength of the medical device itself. The heating temperature is more preferably 105° C. or higher, even more preferably 110° C. or higher, even more preferably 115° C. or higher, and most preferably 121° C. or higher. The heating temperature is more preferably 180° C. or lower, even more preferably 170° C. or lower, and most preferably 150° C. or lower.
[0082] If the heating time is too short, a medical device surface exhibiting good water wettability and slipperiness cannot be obtained, and if it is too long, the strength of the medical device itself is affected, so that the heating time is preferably 5 to 600 minutes. The heating time is more preferably 10 minutes or more, and more preferably 15 minutes or more. The heating time is more preferably 400 minutes or less, and more preferably 300 minutes or less. The heating time in the present invention refers to the time from when the heating temperature is reached to when heating is stopped.
[0083] Sterilization methods in the manufacturing method of the medical device of the present invention include high-pressure steam sterilization, dry heat sterilization, flame sterilization, boiling disinfection, circulating steam disinfection, ethylene oxide gas sterilization (EOG sterilization), radiation sterilization (gamma ray sterilization), ultraviolet sterilization, etc. High-pressure steam sterilization is the most preferable because it can impart excellent water wettability and slipperiness with excellent durability to the base material and from the viewpoint of manufacturing costs. It is preferable to use an autoclave as the apparatus. That is, in the manufacturing method of the medical device of the present invention, it is preferable that the heating is performed by autoclave sterilization (high-pressure steam sterilization using an autoclave).
[0084] After the above sterilization treatment, the obtained medical device may be subjected to other treatments, such as a method of performing the same sterilization treatment again in a solution containing a hydrophilic polymer, a method of replacing the aqueous packaging liquid with an aqueous packaging liquid not containing a hydrophilic polymer and performing the same sterilization treatment, a method of irradiating with radiation, a method of performing an LbL treatment (Layer by Layer treatment) in which polymer materials having opposite charges are alternately coated one layer at a time, a method of performing a crosslinking treatment using metal ions, a method of performing a chemical crosslinking treatment, and the like.
[0085] Furthermore, the substrate may be subjected to a pretreatment prior to the above sterilization treatment, for example, a hydrolysis treatment using an acid such as polyacrylic acid or an alkali such as sodium hydroxide.
[0086] However, in light of the concept of the present invention, which is to impart durable hydrophilicity to the surface of a substrate by a simple method, it is preferable to carry out the treatment within a range that does not make the manufacturing process too complicated.
[0087] The radiation used in the above-mentioned radiation irradiation is preferably various ion beams, electron beams, positron beams, X-rays, gamma rays, or neutron beams, more preferably electron beams and gamma rays, and most preferably gamma rays.
[0088] As the LbL treatment, for example, a treatment using an acidic polymer and a basic polymer as described in WO 2013 / 024800 may be used.
[0089] As the metal ion used in the above-mentioned crosslinking treatment with metal ions, various metal ions are preferable, more preferably monovalent and divalent metal ions, and most preferably divalent metal ions. Chelate complexes may also be used.
[0090] As the above-mentioned chemical crosslinking treatment, for example, a reaction between an epoxy group and a carboxyl group as described in JP-A-2014-533381 or a crosslinking treatment formed with a known acidic hydrophilic polymer having a hydroxyl group may be used.
[0091] In the method of replacing the above solution with a solution not containing a hydrophilic polymer and carrying out the same sterilization treatment, the solution not containing a hydrophilic polymer is not particularly limited, but is preferably a buffer solution. As the buffer, the above-mentioned ones can be used.
[0092] The pH of the buffer solution is preferably in the physiologically acceptable range of 6.3 to 7.8. The pH of the buffer solution is preferably 6.5 or higher, more preferably 6.8 or higher. The pH of the buffer solution is preferably 7.6 or lower, more preferably 7.4 or lower.
[0093] In addition, in the method for producing a medical device of the present invention, since the hydrophilic polymer can impart excellent durability and good water wettability to the substrate, it is preferable that the medical device has a hydrophilic polymer layer on at least a part of the substrate. Having a hydrophilic polymer layer on at least a part of the substrate means, for example, that a polymer layer is present on the entire surface of one side of the substrate surface, depending on the application. In the case where the substrate has no thickness or has a two-dimensional shape with a negligible thickness, it is also preferable that a polymer layer is present on the entire surface of one side of the substrate surface. It is also preferable that a polymer layer is present on the entire surface of the substrate.
[0094] In addition, the hydrophilic polymer is preferably free of covalent bonds with the substrate, since it can be produced in a simple process regardless of whether the substrate is hydrophilic or non-hydrophilic. The absence of covalent bonds is determined by the absence of chemically reactive groups or groups generated by reaction of the chemically reactive groups. Specific examples of chemically reactive groups include, but are not limited to, azetidinium groups, epoxy groups, isocyanate groups, aziridine groups, azlactone groups, and combinations thereof.
[0095] The thickness of the hydrophilic polymer layer is preferably 1 nm or more and less than 100 nm when the vertical cross section of the device in a dry state is observed using a transmission electron microscope. When the thickness is within this range, functions such as water wettability and easy slippage are easily exhibited. The thickness is more preferably 5 nm or more, and even more preferably 10 nm or more. The thickness is more preferably 95 nm or less, even more preferably 90 nm or less, even more preferably 85 nm or less, even more preferably 50 nm or less, even more preferably 30 nm or less, even more preferably 20 nm or less, even more preferably 15 nm or less, and particularly preferably 10 nm or less. If the thickness of the hydrophilic polymer layer is less than 100 nm, it has excellent water wettability and easy slippage, and when used in a medical device such as an ophthalmic lens, for example, the refraction of light for focusing on the retina is not disturbed and poor visibility is unlikely to occur.
[0096] In addition, in the method for producing a medical device of the present invention, the medical device preferably exists in a state in which at least a part of the hydrophilic polymer layer is mixed with the substrate. The state in which the hydrophilic polymer layer is mixed with the substrate can be confirmed by detecting an element derived from the substrate in at least a part of the cross-sectional structure of the substrate and the hydrophilic polymer layer before and after the formation of the hydrophilic polymer layer when the cross-section of the medical device is observed by an observation means capable of performing elemental analysis or composition analysis, such as scanning transmission electron microscopy, electron energy loss spectroscopy, energy dispersive X-ray spectroscopy, and time-of-flight secondary ion mass spectrometry. By mixing the hydrophilic polymer layer with the substrate, the hydrophilic polymer can be more firmly fixed to the substrate.
[0097] When at least a part of the hydrophilic polymer layer is present in a state of being mixed with the substrate, it is preferable to observe a two-layer structure consisting of "a layer in which at least a part of the hydrophilic polymer layer is mixed with the substrate" (hereinafter, mixed layer) and "a layer made of hydrophilic polymer" (hereinafter, single layer). The thickness of the mixed layer is preferably 3% or more, more preferably 5% or more, and even more preferably 10% or more, based on the total thickness of the mixed layer and the single layer. The thickness of the mixed layer is preferably 98% or less, more preferably 95% or less, even more preferably 90% or less, and particularly preferably 80% or less, based on the total thickness of the mixed layer and the single layer. When the thickness ratio of the mixed layer is 3% or more, the hydrophilic polymer and the substrate are sufficiently mixed, and the hydrophilic polymer can be firmly fixed to the substrate, which is preferable. In addition, when the thickness ratio of the mixed layer is 98% or less, it is preferable because the hydrophilicity of the hydrophilic polymer is easily expressed sufficiently.
[0098] In the medical device manufacturing method of the present invention, when the medical device is, for example, a medical device used by being attached to the surface of a living body or an ophthalmic device such as an ophthalmic lens, it is preferable that the liquid film retention time on the surface of the medical device is long, from the viewpoint of preventing the medical device from sticking to the user's skin, etc., and from the viewpoint of preventing the medical device from sticking to the wearer's cornea.
[0099] Here, the liquid film retention time in the present invention refers to the time during which the liquid film on the surface is retained when the medical device is left to stand and immersed in the phosphate buffer solution, then pulled out of the phosphate buffer solution and held in the air. More specifically, it refers to the time during which the liquid film on the surface of the medical device is retained without breaking when the medical device, which has been left to stand and immersed in the phosphate buffer solution, is pulled out of the solution and held in the air with the surface vertical. Note that "the liquid film breaks" refers to a state in which the surface of the medical device repels water.
[0100] In the method for producing a medical device of the present invention, when the medical device is immersed in a phosphate buffer solution and then pulled out of the phosphate buffer solution and held in the air, the time during which the liquid film on the surface is held (liquid film holding time) is preferably 10 seconds or more, more preferably 15 seconds or more, and even more preferably 20 seconds or more. There are no particular limitations on the upper limit of the liquid film holding time, but if the liquid film holding time is too long, water evaporation from the medical device surface is likely to proceed and the effect of the hydrophilic polymer layer will be reduced, so that the upper limit is preferably 300 seconds or less, and more preferably 200 seconds or less.
[0101] In the prior art, even medical devices with good water wettability tended to have extremely low water wettability after scrubbing, and the water wettability that had decreased once did not recover even after leaving the device in water at room temperature for a short time (e.g., about 2 hours). In other words, the decrease in water wettability was observed, which is thought to be caused by the hydrophilic polymer on the substrate surface peeling off or elution due to scrubbing. Therefore, medical devices whose water wettability decreases after scrubbing are not preferable because there is a risk that the surface condition will change due to external stimuli and the water wettability will decrease. Conversely, those whose surface water wettability does not decrease even after scrubbing, or those whose surface water wettability decreases but recovers in a short time, can be said to be excellent medical devices whose surface condition is less likely to change due to external stimuli.
[0102] In the method for producing a medical device of the present invention, when the medical device is an ophthalmic device such as an ophthalmic lens, it is preferable that the liquid film retention time on the surface of the medical device after scrubbing is long, from the viewpoint of reducing the sensation of dryness and maintaining a good wearing comfort for a long period of time.
[0103] Specifically, the medical device is scrubbed with a finger 50 times, and then immersed in a phosphate buffer solution at room temperature for 2 hours, and the liquid film retention time on the surface of the medical device is evaluated. If the liquid film retention time on the surface of the medical device after 2 hours is 10 seconds or more, it means that the surface of the medical device has sufficient water wettability and durability. The liquid film retention time is preferably 10 seconds or more, more preferably 15 seconds or more, and particularly preferably 20 seconds or more. In particular, if the liquid film retention time is the same as before scrubbing, it is preferable because it shows better durability. The details of the measurement method will be described later.
[0104] In addition, in the method for producing a medical device of the present invention, when the medical device is, for example, a medical device that is inserted into a living body and used, it is preferable that the surface of the medical device has excellent slipperiness. As an index of slipperiness, the friction coefficient measured by the method shown in the examples of this specification is preferably small. The friction coefficient is preferably 0.700 or less, more preferably 0.500 or less, and particularly preferably 0.300 or less. In addition, since extremely small friction tends to make handling difficult when putting on and taking off, the friction coefficient is preferably 0.001 or more, more preferably 0.002 or more.
[0105] In the manufacturing method of the medical device of the present invention, the tensile modulus of the medical device should be appropriately selected according to the type of medical device, and in the case of soft medical devices such as ophthalmic lenses, the tensile modulus is preferably 10 MPa or less, more preferably 5 MPa or less, more preferably 3 MPa or less, even more preferably 2 MPa or less, even more preferably 1 MPa or less, and most preferably 0.6 MPa or less. In addition, the tensile modulus is preferably 0.01 MPa or more, more preferably 0.1 MPa or more, even more preferably 0.2 MPa or more, and most preferably 0.25 MPa or more. In the case of soft medical devices such as ophthalmic lenses, if the tensile modulus is too small, it tends to be too soft and difficult to handle. If the tensile modulus is too large, it tends to be too hard and poor wearing and fitting feeling.
[0106] In the method for producing a medical device of the present invention, the change rate of the tensile modulus of the substrate before and after the heating step is preferably 15% or less, more preferably 14% or less, and particularly preferably 13% or less. If the change rate of the tensile modulus of the substrate is too large, it is not preferable because it may cause deformation or poor usability. The details of the measurement method will be described later.
[0107] In the method for producing a medical device of the present invention, the antifouling property of the medical device can be evaluated by lipid (methyl palmitate) adhesion. The less the amount of adhesion as determined by these evaluations, the better the usability and the lower the risk of bacterial proliferation, which is preferable. The details of the measurement method will be described later.
[0108] In the method for producing a medical device of the present invention, it is preferable that the change in moisture content of the medical device obtained after the heating step is 10 percentage points or less compared to the moisture content of the substrate before the heating step, where the change in moisture content (percentage points) refers to the difference in moisture content (% by mass) between the obtained medical device and the moisture content (% by mass) of the substrate from which it is made.
[0109] When used in an ophthalmic device such as an ophthalmic lens, the change in water content of the substrate before and after the heating step is preferably 10 percentage points or less, more preferably 8 percentage points or less, and particularly preferably 6 percentage points or less, from the viewpoint of preventing poor visibility and deformation caused by distortion of the refractive index due to the increase in water content. The details of the measurement method will be described later.
[0110] In addition, when the substrate is used in an ophthalmic device such as an ophthalmic lens, the size change rate of the substrate before and after the heating step is preferably 5% or less, more preferably 4% or less, and particularly preferably 3% or less, from the viewpoint of preventing corneal damage due to deformation. The measurement method will be described later in detail. EXAMPLES
[0111] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. First, analytical and evaluation methods will be described.
[0112] <Water wettability (liquid film retention time)> In order to eliminate the influence of the hydrophilic polymer in the aqueous packaging solution that was not adsorbed to the medical device, the medical device was left to stand in 3 mL of phosphate buffer in a glass vial at room temperature for more than one hour. For the evaluation of only the commercially available contact lens described in the comparative example, the medical device was left to stand in 3 mL of phosphate buffer in a glass vial at room temperature for more than one hour in order to eliminate the influence of the hydrophilic polymer in the packaging solution that was not adsorbed to the lens.
[0113] The medical device was removed from the phosphate buffer solution in which it had been immersed and held in the air, and the time the liquid film on the surface was maintained when the device was visually observed. The average value of N=3 was evaluated according to the following criteria. A: The liquid film on the surface is maintained for more than 20 seconds. B: The liquid film on the surface disappears in 15 to 20 seconds. C: The liquid film on the surface disappears in 10 to 15 seconds. D: The liquid film on the surface disappears in 1 second or more but less than 10 seconds. E: The liquid film on the surface disappears instantly (less than 1 second).
[0114] <Water wettability 2 hours after scrubbing (liquid film retention time)> In order to eliminate the influence of the hydrophilic polymer in the aqueous packaging solution that is not adsorbed to the medical device, the medical device was left in 3 mL of phosphate buffer solution in a glass vial at room temperature for 1 hour. For the evaluation of only the commercially available contact lens described in the comparative example, the medical device was left in 3 mL of phosphate buffer solution in a glass vial at room temperature for 1 hour to eliminate the influence of the hydrophilic polymer in the packaging solution that is not adsorbed to the lens.
[0115] Thereafter, the lens was held between the thumb and index finger and rubbed 50 times, after which it was placed back into the phosphate buffer solution in which it had been left to stand for 2 hours.
[0116] The medical device was removed from the phosphate buffer solution in which it had been immersed and held in the air, and the time the liquid film on the surface was maintained when the device was visually observed. The average value of N=3 was evaluated according to the following criteria. A: The liquid film on the surface is maintained for more than 20 seconds. B: The liquid film on the surface disappears in 15 to 20 seconds. C: The liquid film on the surface disappears in 10 to 15 seconds. D: The liquid film on the surface disappears in 1 second or more but less than 10 seconds. E: The liquid film on the surface disappears instantly (less than 1 second).
[0117] <Moisture content of substrate and medical device> The substrate was immersed in a phosphate buffer solution and left to stand at room temperature for 24 hours or more. The substrate was removed from the phosphate buffer solution, the surface moisture was wiped off with a wiping cloth ("Kimwipe (registered trademark)" manufactured by Nippon Paper Crecia), and the mass (Ww) of the substrate was measured. The substrate was then dried in a vacuum dryer at 40°C for 2 hours, and the mass (Wd) was measured. From these masses, the moisture content of the substrate was calculated using the following formula (1). When the obtained value was less than 1%, it was judged to be below the measurement limit and was expressed as "less than 1%". The average value of N=3 was taken as the moisture content. The moisture content of the substrate after sterilization, i.e., the medical device, was also calculated in the same manner. Moisture content of substrate (%) = 100 × (Ww-Wd) / Ww Equation (1).
[0118] <Change in moisture content of substrate before and after sterilization> From the measurement results of the moisture content of the substrate and the medical device, the change in moisture content was calculated according to the following formula (2). Change in moisture content of substrate before and after sterilization (percentage points) = moisture content of medical device (mass%) - moisture content of substrate (mass%) Formula (2).
[0119] <Coefficient of friction> The friction coefficient of the surface of the medical device wetted with phosphate buffer solution was measured under the following conditions (N=5), and the average value was recorded as the friction coefficient. Equipment: Friction Tester KES-SE (manufactured by Kato Tech Co., Ltd.) Friction SENS:H Measurement speed: 2×1mm / sec Friction load: 44g.
[0120] <Amount of lipid attached> 0.03 g of methyl palmitate, 10 g of pure water, and one contact lens-shaped sample were placed in a 20 cc screw tube. The screw tube was shaken for 3 hours at 37°C and 165 rpm. After shaking, the sample in the screw tube was scrubbed with 40°C tap water and household liquid detergent (Lion's "Mama Lemon (registered trademark)"). The washed sample was placed in a screw tube containing phosphate buffer and stored in a refrigerator at 4°C for 1 hour. The sample was then visually observed, and if there was a cloudy area, it was determined that methyl palmitate was attached, and the area of the part where methyl palmitate was attached relative to the entire surface of the sample was observed.
[0121] <Tensile modulus> Test pieces with a width (minimum part) of 5 mm and a length of 14 mm were cut out from the contact lens-shaped and sheet-shaped substrates using a specified punching die. Using the test pieces, a tensile test was performed using a Tensilon RTG-1210 model manufactured by A&D Co., Ltd. The tensile speed was 100 mm / min, and the distance between the grips (initial) was 5 mm. Measurements were performed on both the substrate before sterilization and the medical device after sterilization. Measurements were performed with N=8, and the average value of N=6 excluding the maximum and minimum values was taken as the tensile modulus.
[0122] <Change in tensile modulus of base material before and after sterilization> The tensile elastic modulus of the substrate and medical device was calculated from the measurement results using the following formula (3). The average value of N=6 was taken as the rate of change in tensile elastic modulus before and after sterilization. Change in tensile elastic modulus of the substrate before and after sterilization (%) = (tensile elastic modulus of the medical device after sterilization - tensile elastic modulus of the substrate before sterilization) / tensile elastic modulus of the substrate before sterilization × 100 Equation (3).
[0123] <Size> For the contact lens-shaped and sheet-shaped base materials (N = 3), the diameter was measured and the average value was taken as the size. The size of the base material after sterilization, that is, the medical device, was also measured in the same way.
[0124] <Size change rate before and after sterilization> From the measurement results of the sizes of the above base materials and medical devices, it was calculated by the following formula (4). The average value of N = 3 was taken as the size change rate before and after sterilization.
[0125] Size change rate before and after sterilization (%) = (Size of the device after sterilization - Size of the base material before sterilization) / Size of the base material before sterilization × 100 Formula (4).
[0126] <Molecular weight measurement> The molecular weight of the hydrophilic polymer was measured under the conditions shown below. Device: Prominence GPC system manufactured by Shimadzu Corporation Pump: LC-20AD Autosampler: SIL-20AHT Column oven: CTO-20A Detector: RID-10A Column: GMPWXL manufactured by Tosoh Corporation (inner diameter 7.8 mm × 30 cm, particle size 13 μm) Solvent: Water / methanol = 1 / 1 (with 0.1 N lithium nitrate added) Flow rate: 0.5 mL / min Measurement time: 30 minutes Sample concentration: 0.1 - 0.3 mass% Sample injection volume: 100 μL Standard sample: Polyethylene oxide standard sample (0.1 kD - 1258 kD) manufactured by Agilent.
[0127] <pH measurement method> The pH of the solution was measured using a pH meter Eutech pH2700 (manufactured by Eutech Instruments). In the table, the pre-sterilization pH of the aqueous packaging solution containing the hydrophilic polymer was measured after adding all of the hydrophilic polymer to the solution described in each Example and Comparative Example, stirring the solution at room temperature (20 to 23°C) for 30 minutes using a rotator to make it uniform. In the table, the "post-sterilization pH" is the pH measured immediately after cooling the solution to room temperature (20 to 23°C) after one sterilization treatment.
[0128] <Determination of Separation of Hydrophilic Polymer Layer> Whether or not the hydrophilic polymer layer was separated was determined by observing a cross section of the medical device using a transmission electron microscope. Equipment: Transmission electron microscope Conditions: Acceleration voltage 100 kV Sample preparation: Samples were prepared by ultrathin sectioning using RuO4 staining. If it is difficult to distinguish between the substrate and the hydrophilic polymer layer, OsO4 staining may be added. In this example, RuO4 staining was used when the substrate was a silicone hydrogel or silicone-based substrate. Ultrathin sections were prepared using an ultramicrotome.
[0129] <Elemental composition analysis of hydrophilic polymer layer> Elemental composition analysis of the hydrophilic polymer layer was performed by analyzing cross-sections of the medical device, which had been frozen in a hydrated state using a cryotransfer holder, with scanning transmission electron microscopy and electron energy loss spectroscopy. Equipment: Field emission electron microscope Acceleration voltage: 200kV Measurement temperature: about -100℃ Electron Energy Loss Spectroscopy: GATAN GIF Tridiem Image acquisition: Digital Micrograph Sample preparation: Samples were prepared by ultrathin sectioning using RuO4 staining. If it is difficult to distinguish between the substrate and the coating layer, OsO4 staining may be added. In this example, RuO4 staining was used when the substrate was a silicone hydrogel or silicone-based substrate. Ultrathin sections were prepared using an ultramicrotome.
[0130] <Film thickness of hydrophilic polymer layer> The cross section of the dry medical device was observed using a transmission electron microscope. Measurements were performed under the conditions described above in <Determination of separation of hydrophilic polymer layer>. The film thickness was measured at three different locations, one location per field of view, and the average film thickness of the three locations was recorded. [Production Example 1] 28 parts by mass of polydimethylsiloxane having methacryloyl groups at both ends and represented by formula (M1) (FM7726, JNC Corporation, Mw: 30,000), 7 parts by mass of silicone monomer represented by formula (M2) (FM0721, JNC Corporation, Mw: 5,000), 57.9 parts by mass of trifluoroethyl acrylate ("Viscoat (registered trademark)" 3F, Osaka Organic Chemical Industry Co., Ltd.), 7 parts by mass of 2-ethylhexyl acrylate (Tokyo Chemical Industry Co., Ltd.), and 0.1 parts by mass of dimethylaminoethyl acrylate (Kojin Co., Ltd.), and relative to the total mass of these monomers, 5,000 ppm of photoinitiator "Irgacure (registered trademark)" 819 (Nagase & Co., Ltd.), 5,000 ppm of ultraviolet absorber (RUVA-93, Otsuka Chemical), and 5,000 ppm of colorant (RB246, Arran Chemical (100 ppm) was prepared, and 10 parts by mass of t-amyl alcohol was prepared based on 100 parts by mass of the total mass of the monomers, and all of these were mixed and stirred. The stirred mixture was filtered through a membrane filter (pore size: 0.45 μm) to remove insoluble matter, and a monomer mixture was obtained.
[0131] The above monomer mixture was injected into a contact lens mold made of transparent resin (base curve side material: polypropylene, front curve side material: polypropylene) and irradiated with light (wavelength 405 nm (± 5 nm), illuminance: 0 to 0.7 mW / cm 2 The mixture was then polymerized by heating for 30 minutes to obtain a molded product made of a soft, low water content material containing silicon atoms.
[0132] After polymerization, the obtained molded body, together with the mold from which the front curve and base curve were released, was immersed in a 100% by mass aqueous solution of isopropyl alcohol at 60°C for 1.5 hours, and the contact lens-shaped molded body was peeled off from the mold. The obtained molded body was immersed in a large excess of a 100% by mass aqueous solution of isopropyl alcohol kept at 60°C for 2 hours to extract impurities such as residual monomers. Then, it was dried at room temperature (23°C) for 12 hours.
[0133] [ka]
[0134] <Phosphate buffer solution> The compositions of the phosphate buffer solutions used in the processes of the following Examples and Comparative Examples and in the above-mentioned measurements are as follows: In the compositions below, EDTA2Na stands for disodium dihydrogen ethylenediaminetetraacetate. KCl 0.2g / L KH2PO40.2g / L NaCl 8.0g / L Na2HPO41.19g / L EDTA2Na 0.5g / L.
[0135] [Example 1] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.05% by mass of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 280,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0136] [Example 2] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.05% by mass of poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0137] [Example 3] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a phosphate buffer solution containing 0.04% by mass of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 280,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.), and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0138] [Example 4] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.04% by mass of poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0139] [Example 5] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.05% by mass of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 280,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device by the above method are shown in Tables 1 to 3.
[0140] [Example 6] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) whose main components are polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.05% by mass of poly N,N-diethylacrylamide (Mw: 290,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device by the above method are shown in Tables 1 to 3.
[0141] [Example 7] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) whose main components are polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.04% by mass of poly N,N-diethylacrylamide (Mw: 290,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device by the above method are shown in Tables 1 to 3.
[0142] [Example 8] The molded article obtained in Production Example 1 was used as the substrate. The substrate was immersed in a solution containing 0.04 mass% of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization: 1 / 9, Mw: 280,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0143] [Example 9] The molded article obtained in Production Example 1 was used as the substrate. The substrate was immersed in a solution containing 0.04% by mass of poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0144] [Example 10] A commercially available PF catheter tube (manufactured and sold by Toray Industries, Inc.) mainly composed of polyurethane was used as the substrate. The substrate was immersed in a solution containing 0.04 mass% of acrylic acid / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 800,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and heated in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0145] [Example 11] A commercially available PF catheter tube (manufactured and sold by Toray Industries, Inc.) mainly composed of polyurethane was used as the substrate. The substrate was immersed in a solution containing 0.04% by mass of poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and heated in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0146] [Example 12] As the substrate, a commercially available film "Mictron (registered trademark)" (manufactured by Toray Industries, Inc.) mainly composed of para-type aromatic polyamide (aramid) was used. The substrate was immersed in a solution containing 0.04 mass% of acrylic acid / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 800,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and heated in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0147] [Example 13] As the substrate, a commercially available film "Mictron (registered trademark)" (manufactured by Toray Industries, Inc.) mainly composed of para-type aromatic polyamide (aramid) was used. The substrate was immersed in a solution containing 0.04 mass% poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and heated in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0148] [Example 14] The substrate used was a commercially available hydrogel lens "1day Acuvue (registered trademark)" (Johnson & Johnson, etafilcon A) mainly composed of 2-hydroxyethyl methacrylate. The substrate was immersed in a solution containing 0.04 mass% of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 280,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0149] [Example 15] The substrate used was a commercially available hydrogel lens "1day Acuvue (registered trademark)" (manufactured by Johnson & Johnson, etafilcon A) whose main component is 2-hydroxyethyl methacrylate. The substrate was immersed in a solution containing 0.04% by mass of poly N,N-diethylacrylamide (Mw: 290,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above method are shown in Tables 1 to 3.
[0150] [Example 16] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.05% by mass of N,N-dimethylacrylamide / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 280,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device by the above method are shown in Tables 1 to 3.
[0151] [Example 17] As the substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was used. The substrate was immersed in a solution containing 0.05 mass% of acrylic acid / N,N-dimethylaminopropylacrylamide methyl chloride quaternary salt / N,N-diethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 8, Mw: 280,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device by the above method are shown in Tables 1 to 3.
[0152] [Example 18] The molded article obtained in Production Example 1 was used as the substrate. The substrate was immersed in a solution containing 0.05% by mass of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization: 1 / 9, Mw: 280,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0153] [Example 19] The molded article obtained in Production Example 1 was used as the substrate. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / N,N-diethylacrylamide copolymer (molar ratio in copolymerization: 1 / 9, Mw: 280,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device by the above-mentioned method are shown in Tables 1 to 3.
[0154] [Table 1-1]
[0155] [Table 1-2]
[0156] [Table 1-3]
[0157] [Table 2-1]
[0158] [Table 2-2]
[0159] [Table 2-3]
[0160] [Table 3-1]
[0161] [Table 3-2]
[0162] [Table 3-3]
[0163] [Comparative Example 1] A commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) containing silicone as the main component was immersed in a phosphate buffer solution and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above-mentioned method are shown in Tables 4 to 6.
[0164] [Comparative Example 2] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / acrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 250,000, self-made) in phosphate buffer, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0165] [Comparative Example 3] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 200,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0166] [Comparative Example 4] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 9, Mw: 800,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0167] [Comparative Example 5] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / acryloylmorpholine copolymer (molar ratio in copolymerization 1 / 9, Mw: 500,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0168] [Comparative Example 6] The substrate used was a commercially available silicone hydrogel lens "MyDay (registered trademark)" (manufactured by CooperVision, stenfilcon A) whose main component is silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / acryloylmorpholine copolymer (molar ratio in copolymerization 1 / 9, Mw: 320,000, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0169] [Comparative Example 7] As the substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was used. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 2, Mw: 550,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0170] [Comparative Example 8] As the substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was used. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 2, Mw: 330,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0171] [Comparative Example 9] As the substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was used. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 8, Mw: 500,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0172] [Comparative Example 10] As the substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was used. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 8, Mw: 370,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0173] [Comparative Example 11] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone copolymer (molar ratio in copolymerization 1 / 4, Mw: 590,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0174] [Comparative Example 12] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / vinylpyrrolidone copolymer (molar ratio in copolymerization 1 / 9, Mw: 390,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (hydrophilic polymer layer not confirmed) by the above method are shown in Tables 4 to 6.
[0175] [Comparative Example 13] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / 2-hydroxyethyl methacrylate / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 2, Mw: 430,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0176] [Comparative Example 14] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03 mass% of acrylic acid / 2-hydroxyethyl methacrylate / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization 1 / 1 / 8, Mw: 480,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained medical device (hydrophilic polymer layer was not confirmed) by the above method are shown in Tables 4 to 6.
[0177] [Comparative Example 15] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03% by mass of polyvinylpyrrolidone (Mw: 360,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0178] [Comparative Example 16] The substrate used was a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone. The substrate was immersed in a solution containing 0.03% by mass of poly N,N-dimethylacrylamide (Mw: 360,000, Osaka Organic Chemical Industry Co., Ltd.) in a phosphate buffer solution, and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0179] [Comparative Example 17] As a substrate, a commercially available silicone hydrogel lens "Acuvue Oasys (registered trademark)" (Johnson & Johnson, senofilcon A) mainly composed of polyvinylpyrrolidone and silicone was immersed in a phosphate buffer solution and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0180] [Comparative Example 18] The molded body obtained in Production Example 1 was used as a substrate and immersed in a phosphate buffer solution and sterilized in an autoclave for 30 minutes at 121° C. The obtained medical device (no hydrophilic polymer layer was observed) was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.
[0181] [Comparative Example 19] As a substrate, a commercially available hydrogel lens "1day Acuvue (registered trademark)" (manufactured by Johnson & Johnson, etafilcon A) mainly composed of 2-hydroxyethyl methacrylate was immersed in a phosphate buffer solution and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0182] The substrate of this comparative example showed a relatively good liquid film retention time and good durability even without the application of the manufacturing method of the present invention. However, compared with Examples 14 and 15 in which the manufacturing method of the present invention was applied to the same substrate, it was shown that the liquid film retention time was significantly improved (from 20 seconds to 120 seconds) by applying the manufacturing method of the present invention.
[0183] [Comparative Example 20] As a substrate, a commercially available PF catheter tube (manufactured and sold by Toray Industries, Inc.) mainly composed of polyurethane was immersed in a phosphate buffer solution and sterilized in an autoclave for 30 minutes at 121° C. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0184] [Comparative Example 21] As a substrate, a commercially available film "Mictron (registered trademark)" (manufactured by Toray Industries, Inc.) mainly composed of para-type aromatic polyamide (aramid) was immersed in a phosphate buffer solution and sterilized in an autoclave at 121°C for 30 minutes. The results of evaluation of the obtained medical device (no hydrophilic polymer layer was observed) by the above method are shown in Tables 4 to 6.
[0185] [Table 4-1]
[0186]
Table 4-2
[0187]
Table 4-3
[0188]
Table 5-1
[0189]
Table 5-2
[0190]
Table 5-3
[0191]
Table 6-1
[0192]
Table 6-2
[0193]
Table 6-3
Claims
1. A method for producing a medical device, comprising the step of heating an aqueous packaging solution, the heating being carried out in a state in which one or more hydrophilic polymers are contained in the aqueous packaging solution and at least a portion of a substrate of the medical device is in contact with the aqueous packaging solution; A method for manufacturing a medical device, which satisfies all of the following requirements (a) to (c): (a) The hydrophilic polymer is a homopolymer of (meth)acrylamide having two substituents with two or more carbon atoms on the nitrogen atom, or a copolymer of (meth)acrylamide having two substituents with two or more carbon atoms on the nitrogen atom and (meth)acrylic acid. (b) the mass % concentration of the hydrophilic polymer contained in the aqueous packaging liquid is in the range of 0.0001 to 30 mass %; (c) the pH of the aqueous packaging solution after the heating step is in the range of 6.1 to 8.0;
2. The method for producing a medical device according to claim 1, wherein a copolymerization ratio of the copolymer of (meth)acrylamide having two substituents each having two or more carbon atoms on a nitrogen atom and (meth)acrylic acid is [mass of (meth)acrylic acid monomer] / [mass of (meth)acrylamide monomer having two substituents each having two or more carbon atoms on a nitrogen atom]=1 / 99 to 99 / 1.
3. The method for producing a medical device according to claim 1 or 2, wherein the heating is carried out by autoclave sterilization.
4. The method for producing a medical device according to any one of claims 1 to 3, wherein the substrate comprises one or more materials selected from the group consisting of hydrogels, silicone hydrogels, low water content soft materials, and low water content hard materials.
5. 5. The method of claim 4, wherein the hydrogel is selected from the group consisting of tefilcon, tetrafilcon, helfilcon, mafilcon, polymacon, hioxifilcon, alfafilcon, omafilcon, nelfilcon, nesofilcon, hilafilcon, acofilcon, deltafilcon, etafilcon, focofilcon, ocufilcon, phemfilcon, methafilcon, and vilfilcon.
6. 5. The method of claim 4, wherein the silicone hydrogel is selected from the group consisting of lotrafilcon, galyfilcon, narafilcon, senofilcon, comfilcon, enfilcon, balafilcon, efrofilcon, fanfilcon, somofilcon, samfilcon, olifilcon, asmofilcon, formofilcon, stenfilcon, abafilcon, mangofilcon, riofilcon, sifilcon, larafilcon, and delefilcon.
7. The method for producing a medical device according to claim 4 , wherein the low water content soft material is a material containing silicon atoms.
8. The method for producing a medical device according to claim 4 , wherein the low water content, hard material is a material containing silicon atoms.
9. The method for producing a medical device according to claim 4 , wherein the low water content hard material is polymethyl methacrylate.
10. The method for producing a medical device according to claim 4, 8 or 9, wherein the low water content hard material is a material selected from the group consisting of neofocon, pasifocon, telefocon, silafocon, paflufocon, petrafocon and fluorofocon.
11. The method for producing a medical device according to any one of claims 1 to 10, wherein the medical device is an ophthalmic lens, a skin covering material, a wound covering material, a skin protective material, a skin drug carrier, an infusion tube, a gas transport tube, a drainage tube, a blood circuit, a covering tube, a catheter, a stent, a sheath, a biosensor chip, an artificial heart-lung machine, or an endoscope covering material.
12. The method of claim 11 , wherein the ophthalmic lens is a contact lens.
Citation Information
Patent Citations
JP1975013059A
Arukaridenchi
JP1976054231A
Surface treatment of medical devices
JP2003535626A
Comfortable ophthalmic device and manufacturing method thereof
JP2008532060A
Silicone hydrogel, lens for eyes, and contact lens
JP2011197196A