Fixing member, fixing device and image forming apparatus
A fixing member with a specific filler orientation and composition in the elastic layer addresses the challenge of high thermal conductivity and deformation resistance, ensuring high-quality image formation and durability.
Patent Information
- Application Number
- JP2020084440
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-23
- Filing Date
- 2020-05-13
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-05-13
AI Technical Summary
Existing fixing members in thermal fixing devices face challenges in achieving high thermal conductivity in the thickness direction without increasing hardness or susceptibility to deformation, especially when used in high-temperature conditions.
A fixing member with an elastic layer containing specific ratios and orientations of inorganic oxide fillers, such as alumina, zinc oxide, and silicon oxide, is developed, where the fillers with major axes less than 1.5 to the minor axes ratio are spherical and those with 1.5 or more are amorphous, oriented at angles between 50° and 90° to the thickness direction, enhancing thermal conductivity while maintaining low hardness.
The solution results in a fixing member with high thermal conductivity, resistance to deformation, and low hardness, enabling the formation of high-quality electrophotographic images with improved paper passing durability.
Smart Images

Figure 0007587357000007 
Figure 0007587357000008 
Figure 0007587357000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a fixing member, a fixing device, and an image forming apparatus used in an electrophotographic image forming apparatus such as a copier or a printer. [Background technology]
[0002] Generally, in a thermal fixing device (hereinafter, simply referred to as a "fixing device") used in an image forming apparatus, a pair of rotating bodies, such as a pair of heated rollers or a pair of heated rollers, are in pressure contact with each other as fixing members. A recording medium carrying an image made of unfixed toner is introduced into the pressure contact area formed between the rotating bodies and heated, melting the toner and fixing the image to the recording medium.
[0003] The members of the fixing device include fixing members, pressure members, etc. The rotating body that comes into contact with the unfixed toner image held on the recording medium is called the fixing member, and is called a fixing roller, a fixing belt, etc. depending on its form. On the other hand, the rotating body that does not come into contact with the unfixed toner image and is on the opposite side across the recording medium is called the pressure member, and is called a pressure roller, a pressure belt, etc. depending on its form.
[0004] A commonly known fixing member has a structure in which an elastic layer containing heat-resistant silicone rubber is disposed on a base formed of a metal or heat-resistant resin, and further coated or formed with a thin layer of fluororesin via an adhesive. The elastic layer of the fixing member is required to have high thermal conductivity as well as elasticity. Therefore, the elastic layer contains an inorganic filler with high thermal conductivity as a thermally conductive filler in rubber such as silicone rubber. However, if the amount of the thermally conductive filler in the elastic layer is increased in order to give the elastic layer higher thermal conductivity, the elastic layer may become hard and the elasticity of the elastic layer may decrease.
[0005] In recent years, there has been a demand for further improving the thermal conductivity in the thickness direction of the elastic layer of the fixing member in order to increase the printing speed, improve the image quality, etc. Therefore, there is a demand for a technology for increasing the thermal conductivity of the elastic layer without excessively increasing the content of the thermally conductive filler. Patent document 1 discloses a fixing member in which the thermally conductive filler contained in the elastic layer is a blend of large particle size filler and small particle size filler, thereby achieving both low hardness and high thermal conductivity in the elastic layer with a relatively small amount of filler. Moreover, Patent Document 2 discloses a fixing roller in which carbon fiber filler is oriented in the thickness direction to provide an elastic layer with high thermal conductivity. Furthermore, Patent Document 3 discloses a resin composition in which a thermally conductive filler is filled in a synthetic resin, and the filler is oriented in the direction of the applied electric field by using an electric field to impart high thermal conductivity without increasing the amount of filler blended. The orientation referred to here means that the long sides of the filler having an aspect ratio are oriented in the direction of the applied electric field. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-300591 A [Patent Document 2] JP 2007-101736 A [Patent Document 3] JP 2013-159748 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, according to the study by the present inventors, in order to make the thermal conductivity of the elastic layer according to Patent Document 1 exceed 1.5 W / (m K), it is considered necessary to make the filler content relative to the silicone rubber 60 volume % or more. In this case, it becomes difficult to achieve a low hardness in order to achieve a further high thermal conductivity. Furthermore, the present inventors achieved a softness of, for example, 15° in JIS A hardness (JIS K6253) by setting the volumetric blending amount of the filler to more than 50% by volume and reducing the amount of the crosslinking agent in the elastic layer according to Patent Document 1. As a result, when such an elastic layer is repeatedly compressed in a state where it is heated to a high temperature such as 200° C., the elastic layer may break or undergo plastic deformation. Furthermore, in the invention of Patent Document 2, the thickness of the elastic layer needs to be about 1 to 5 mm in order to orient the carbon fibers in the thickness direction, and it is difficult to improve the thermal conductivity of a fixing member having a thin elastic layer of 500 μm or less. Furthermore, when the technology disclosed in Patent Document 3 was applied to the elastic layer of the fixing member, all of the filler that was mixed in the state shown in FIG. 1(a) before orientation was oriented in the thickness direction, resulting in the filler orientation state shown in FIG. 1(b). As a result, the hardness increased, and the elastic layer had areas with sparse and dense fillers, resulting in uneven hardness. Therefore, it was difficult to apply this technology to the fixing member. One aspect of the present disclosure is to provide a fixing member having a low hardness elastic layer that has high thermal conductivity in the thickness direction, is resistant to fracture or plastic deformation even when repeatedly compressed at high temperatures. Another aspect of the present disclosure is directed to providing a thermal fixing device that contributes to the formation of high-quality electrophotographic images. Still another aspect of the present disclosure is directed to providing an image forming apparatus that can form high-quality electrophotographic images. [Means for solving the problem]
[0008] According to one aspect of the present disclosure, there is provided a fixing member that fixes an unfixed toner image formed on a recording medium as a fixed image by applying pressure and heat to the recording medium, the fixing member comprising: A substrate; and an elastic layer on the outer periphery of the substrate, the elastic layer including a filler including an inorganic oxide, The filler includes at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, and silicon oxide; (1) A binary image of a first cross section of the elastic layer in the thickness-circumferential direction and a binary image of a second cross section of the elastic layer in the thickness-axial direction, When the shape of the filler is approximated as an ellipse, The area ratio of the first filler having a major axis / minor axis ratio of less than 1.5 is A; When the area ratio of the second filler having a major axis / minor axis ratio of 1.5 or more is B, 1.0≦(A / B)≦2.0 and 0.40≦(A+B)≦0.50, (2) The average orientation angle θAve of the second filler having a major axis / minor axis ratio of 1.5 or more with respect to the thickness direction of the elastic layer is 50°≦θAve ≦90°. in can be, the first filler is a spherical inorganic oxide, The second filler is an amorphous inorganic oxide. A fuser member is provided.
[0009] According to another aspect of the present disclosure, there is provided a thermal fixing device having the fixing member described above. Furthermore, according to another aspect of the present disclosure, there is provided an image forming apparatus having a photoconductor, a charging device for charging the photoconductor, an exposure device for exposing the charged photoconductor to light to form an electrostatic latent image, a developing device for developing the electrostatic latent image formed on the photoconductor with toner to form a toner image, a transfer device for transferring the toner image formed on the photoconductor to a recording medium, and the above-mentioned thermal fixing device. Effect of the Invention
[0010] According to one aspect of the present disclosure, there is provided a fixing member having a low hardness elastic layer that has high thermal conductivity in the thickness direction and is resistant to fracture or plastic deformation even when repeatedly compressed at high temperatures. According to another aspect of the present disclosure, there is provided a thermal fixing device and an image forming apparatus that have excellent fixing properties, can form high-quality electrophotographic images, and have excellent paper feed durability. [Brief description of the drawings]
[0011] [Figure 1]1A and 1B are conceptual diagrams illustrating the dispersion state of filler in an elastic layer of a conventional fixing member, where (a) shows a non-oriented state of the filler, and (b) shows an example of a conventional oriented state of the filler. [Diagram 2] 1A and 1B are conceptual diagrams illustrating the dispersion state of a filler in an elastic layer in the present disclosure, in which (a) is an example of a filler unoriented state and (b) is an example of a filler oriented state. [Diagram 3] FIG. 2 is a conceptual diagram relating to an orientation torque applied to a filler in an elastic layer. [Figure 4] 1A and 1B are schematic cross-sectional views of fixing members according to an embodiment of the present disclosure, where (a) shows a belt configuration and (b) shows a roller configuration. [Diagram 5] 2A and 2B are an overhead view and a cross-sectional view of a corona charger for forming an elastic layer of a fixing member according to an embodiment of the present disclosure. [Figure 6] 5A and 5B are diagrams illustrating a first cross section and a second cross section of the elastic layer of the roller-type fixing member illustrated in FIG. [Figure 7] FIG. 2 is a schematic diagram showing a method for confirming the average orientation angle θAve of a filler in an elastic layer. [Figure 8] FIG. 2 is a schematic diagram of an example of a step of laminating a surface layer. [Figure 9] FIG. 2 is a schematic cross-sectional view showing an example of a thermal fixing device using a fixing belt and a pressure belt. [Figure 10] FIG. 2 is a schematic cross-sectional view showing an example of a fixing belt pressure roller type thermal fixing device. [Figure 11] FIG. 2 is a schematic diagram relating to a high-temperature pressure test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The fixing member, the thermal fixing device, and the image forming apparatus according to the present disclosure will be described in detail below with reference to the drawings. However, the technical scope of the present disclosure is not limited to the following exemplary embodiments. The present inventors have conducted research aimed at obtaining a fixing member having an elastic layer with high thermal conductivity in the thickness direction, which is resistant to fracture or plastic deformation even when repeatedly compressed at high temperatures, and low hardness. As a result, they have found that an elastic layer in which a thermally conductive filler is dispersed in a specific state is effective in achieving the above-mentioned objective.
[0013] The fixing member according to the present disclosure comes into contact with an unfixed toner image and heats the unfixed toner image in a fixing device that heats an unfixed toner image on a recording medium with an electrophotographic fixing member to fix the unfixed toner image on the recording medium. The fixing member includes at least a substrate and an elastic layer including a filler including an inorganic oxide provided on the outer periphery of the substrate, the filler including at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, and silicon oxide, (1) A binary image of a first cross section of the elastic layer in the thickness-circumferential direction and a binary image of a second cross section of the elastic layer in the thickness-axial direction, When the shape of the filler is approximated as an ellipse, The area ratio of a filler containing an inorganic oxide having a major axis / minor axis ratio (major axis / minor axis) of less than 1.5 (hereinafter also referred to as "first filler") is A, When the area ratio of the filler containing an inorganic oxide having a long axis / short axis ratio of 1.5 or more (hereinafter also referred to as the "second filler") is B, 1.0≦(A / B)≦2.0 and 0.40≦(A+B)≦0.50, (2) The average orientation angle θAve of the second filler with respect to the thickness direction of the elastic layer having a major axis / minor axis ratio of 1.5 or more is 50°≦θAve≦90°. in can be, the first filler is a spherical inorganic oxide, The second filler is an amorphous inorganic oxide. be.
[0014] The thermal conductivity of the elastic layer in the thickness direction is preferably 1.3 W / (m·K) or more and less than 2.0 W / (m·K). The major axis / minor axis and average orientation angle θ when the filler shape is approximated as an ellipse AveThe area percentage can be determined by image processing described later. The area percentage is synonymous with the volume % of the filler content.
[0015] 2(b), the elastic layer according to the present disclosure includes a first filler having a ratio of major axis to minor axis (major axis / minor axis) of less than 1.5 when the shape of the filler observed from the first cross section and the second cross section of the elastic layer is approximated as an ellipse, and a second filler having a ratio of major axis to minor axis of 1.5 or more. In this specification, the ratio of major axis to minor axis (major axis / minor axis) may be referred to as the "aspect ratio". The second filler having an aspect ratio of 1.5 or more has an average orientation angle θ in the thickness direction of the elastic layer. Ave However, 50°≦θ Ave ≦90°. This allows the thermal conductivity in the thickness direction to be sufficiently increased without excessively increasing the total filler content in the elastic layer. In addition, by reducing the total filler content, it is possible to prevent an excessive increase in the hardness of the elastic layer. As a result, it is possible to obtain an elastic layer that has both high thermal conductivity in the thickness direction and low hardness. In addition, in Figures 1 and 2, the vertical direction of the figures is the thickness direction of the elastic layer. As a method for ellipse approximation, approximation by the least squares method can be used.
[0016] A silicone rubber composition containing a first filler with an aspect ratio of less than 1.5 can reduce local stress generated at the interface between the filler and the silicone rubber, regardless of the direction of pressure, compared to a silicone composition containing a second filler with an aspect ratio of 1.5 or more. In an elastic layer in which the "A / B" is within the range of 1.0 to 2.0, the amount of the first filler in the elastic layer is considered to be equal to or greater than the amount of the second filler. As a result, even if a large strain is applied to the elastic layer, the stress concentration at least near the interface between the first filler and the silicone rubber is reduced, and fracture or plastic deformation from the interface between the filler and the silicone rubber is considered to be effectively suppressed.
[0017] On the other hand, as a method for increasing the thermal conductivity in the thickness direction without increasing the amount of the thermally conductive filler blended in the elastic layer, there is a technique for orienting the filler by an external field such as a force field, a magnetic field, or an electric field. The materials generally used as the thermally conductive filler to be blended in the elastic layer of the fixing member are often amorphous inorganic oxides such as alumina, silica, zinc oxide, and magnesium oxide, which have a high affinity for orientation by an electric field using dielectric polarization as a driving force. The electric field orientation technology disclosed in Patent Document 3 involves sandwiching a curable liquid in which a thermally conductive filler is dispersed between parallel plate electrodes, applying an AC electric field for several tens of minutes to several hours, and simultaneously curing the liquid with heat or the like. This causes the filler to undergo dielectrophoresis, thereby obtaining a cured product in which the filler is oriented in the direction between the electrodes. However, in the above-mentioned method, as shown in FIG. 1(b), all of the blended filler is oriented in the thickness direction, which may lead to an increase in hardness or unevenness in hardness.
[0018] In contrast, in the elastic layer of the fixing member according to the present disclosure, which is formed through a charge application process to the outer surface of the uncured rubber composition layer described below, the first filler having a long axis / short axis ratio of less than 1.5 has a low degree of orientation in the thickness direction of the elastic layer. On the other hand, the second filler having a major axis / minor axis ratio of 1.5 or more rotates and is oriented by the orientation torque due to dielectric polarization as shown in FIG. 3 by the process of applying electric charge to the outer surface of the uncured elastic layer. As a result, the second filler having a major axis / minor axis ratio of 1.5 or more changes from the dispersion state shown in FIG. 2(a) to the dispersion state shown in FIG. 2(b). Therefore, in the cured elastic layer, the thermal conductivity is further improved due to the thermal conduction path formed by the oriented second filler having a major axis / minor axis ratio of 1.5 or more. This makes it possible to increase the high thermal conductivity in the thickness direction while suppressing the increase in the content of the thermally conductive filler in the elastic layer. As a result, the flexibility of the elastic layer is also maintained.
[0019] The elastic layer according to the present disclosure can be manufactured, for example, by the following method. After forming a rubber composition layer containing a thermally conductive filler and uncured rubber on a substrate, the surface of the rubber composition layer is charged before the rubber composition layer is cured. As a result, the filler contained in the rubber composition layer, which is mainly amorphous and has a large aspect ratio, is dielectrically polarized and oriented under torque. As a method of charging, a non-contact method is preferable, and more preferably, a corona charger capable of approximately uniform charging in a simple and inexpensive manner is preferable. The composition layer is then cured, resulting in the formation of an elastic layer in which the fillers having a large aspect ratio are oriented in the thickness direction and in which heat conduction paths for efficient heat transfer are formed.
[0020] In the elastic layer according to the present disclosure, the mechanism by which the second filler particles having a major axis / minor axis ratio of 1.5 or more selectively move and are oriented as shown in FIG. 2(b) instead of being oriented overall as shown in FIG. 1(b) is unclear, but is speculated as follows. That is, in a system in which the elastic layer is sandwiched between parallel plate electrodes and an electric field is applied, the electric field from the electrodes causes the entire filler to undergo dielectrophoresis. In contrast, in this embodiment, the electric field is applied by, for example, charging the elastic layer in a short time without contacting the elastic layer using a corona charger. It is speculated that this does not exert a force strong enough to dielectrophoretically cause the first filler particles having a major axis / minor axis ratio of less than 1.5. A fixing member and a thermal fixing device according to an embodiment of the present disclosure will be described in detail below based on a specific configuration.
[0021] (1) Overview of the fixing member structure The fixing member according to one embodiment of the present disclosure will be described in detail with reference to the drawings. 4(a) and 4(b) are schematic cross-sectional views showing the fixing member according to this embodiment. Fig. 4(a) shows a cross section in a direction perpendicular to the circumferential direction of a fixing member having an endless shape (hereinafter also referred to as a "fixing belt"), and Fig. 4(b) shows a cross section in a direction perpendicular to the circumferential direction of a fixing member having a roller shape (hereinafter also referred to as a "fixing roll"). Note that the endless shape is a shape in which the fixing belt rotates in the circumferential direction so that the same part can pass through the fixing nip portion multiple times (endlessly). 4(a) and 4(b), an elastic layer 4 containing silicone rubber as a binder covers the outer circumferential surface of a substrate 3. In Fig. 4(a) and 4(b), the radial direction is the thickness direction of the elastic layer. Thus, the fixing member according to this embodiment has a substrate 3 and an elastic layer 4 on the substrate 3, the elastic layer 4 including silicone rubber.
[0022] As shown in these figures, the fixing member may have a surface layer 6 on an elastic layer 4 that includes silicone rubber. The fixing member may also have an adhesive layer 5 between the elastic layer 4 containing silicone rubber and the surface layer 6, in which case the surface layer 6 is fixed to the outer peripheral surface of the elastic layer 4 containing silicone rubber by the adhesive layer 5.
[0023] (2) Substrate of the fixing member The substrate 3 used in the fixing belt shown in FIG. 4(a) may be an endless substrate containing a metal such as nickel or stainless steel, or an endless substrate containing a resin such as polyimide. Here, when an electromagnetic induction heating method is used to heat the fixing belt, a substrate containing mainly nickel or iron, which has high heat generation efficiency, is preferably used. A layer for imparting a function of improving adhesion to the elastic layer can be provided on the outer surface (the surface on the elastic layer side) of the base 3. That is, the elastic layer 4 only needs to be provided on the outer peripheral surface of the base 3, and another layer can be provided between the elastic layer 4 and the base 3. Also, a layer for imparting a function such as wear resistance or lubricity can be further provided on the inner surface (the surface opposite to the outer surface) of the base 3. When the base 3 is in the form of a belt, a core is inserted inside the sleeve during the following manufacturing process.
[0024] The base 3 used in the fixing roller shown in FIG. 4(b) may be a mandrel (hereinafter also referred to as a core metal) made of a metal or alloy such as aluminum or iron. The base 3 used in the fixing roller is required to have a strength sufficient to withstand the pressure applied when a pressure member is pressed against the fixing roller in a thermal fixing device. The base 3 of the fixing roll shown in FIG. 4(b) is a solid core metal, but a hollow mandrel can also be used. When a hollow mandrel is used, a heat source such as a halogen lamp can be placed inside it.
[0025] (3-1) Elastic layer containing silicone rubber The elastic layer 4 containing silicone rubber functions as a layer that imparts excellent flexibility so that the fixing member can follow the unevenness of the paper during fixing. Silicone rubber is preferable because it has high heat resistance that allows it to maintain flexibility even in an environment where the temperature reaches a high temperature of about 240°C in the non-paper passing area. In addition, silicone rubber is preferably electrically insulating because the surface is charged before the rubber hardens to orient the filler. As such silicone rubber, for example, a cured product of addition-curing liquid silicone rubber can be used as described later.
[0026] The elastic layer 4 containing silicone rubber contains a thermally conductive filler in order to improve the thermal conductivity in the thickness direction of the elastic layer. The type of filler is selected taking into consideration the thermal conductivity, specific heat capacity, density, particle size, shape, and relative dielectric constant of the filler itself. 2 O 3), zinc oxide (ZnO), magnesium oxide (MgO), silica (SiO 2 These fillers may be used alone or in combination. In addition, metal fillers and carbon fiber fillers have low electrical resistance and are therefore unlikely to cause dielectric polarization when an electric field is applied, making them unsuitable for use alone, unless the electrical resistance can be controlled by surface treatment to form an oxide film.
[0027] The filler may be surface-treated from the viewpoint of obtaining a desired affinity for the silicone base material and a desired electrical resistance value. Specifically, fillers such as alumina, silica, and magnesium oxide that have active groups such as hydroxyl groups on the surface are surface-treated with a silane coupling agent, hexamethyldisilazane, or the like.
[0028] Among the fillers containing an inorganic oxide in the elastic layer, when the shape of the filler is approximated as an ellipse, the area ratio of a first filler having a major axis / minor axis ratio of less than 1.5 is defined as A, and the area ratio of a second filler having a major axis / minor axis ratio of 1.5 or more is defined as B. 1.0≦(A / B)≦2.0, and 0.40≦(A+B)≦0.50 It is.
[0029] As described above, when (A / B) is 1.0 to 2.0, even if a large strain is applied to the elastic layer, destruction from the interface between the filler and the silicone rubber or plastic deformation of the elastic layer is unlikely to occur. Therefore, the elastic layer can exhibit high durability. This is believed to be because the filler having a shape close to a sphere, with a major axis / minor axis ratio of less than 1.5, is contained at a predetermined ratio relative to the total filler, and therefore, even if a strain is applied to the elastic layer from any direction, the local stress generated at the interface between the filler and the silicone rubber is alleviated.
[0030] In addition, among the fillers in the elastic layer according to the present embodiment, the second filler having a major axis / minor axis ratio of 1.5 or more has an average orientation angle θ Ave However, 50°≦θ Ave≦90°。 This makes it possible to increase the thermal conductivity in the thickness direction without excessively increasing the total filler content in the elastic layer. As a result, it is possible to obtain a fixing member with increased thermal conductivity in the thickness direction without excessively increasing the hardness of the elastic layer.
[0031] The area proportions A and B of each filler group in the elastic layer are ratios to the volume of the mixture of silicone rubber and filler (elastic layer), and indicate values of 0 to 1 (0 to 100 volume %). The area ratio (A / B) of each filler group in the elastic layer is set to be 1 or more and 2 or less. If A / B is less than 1, durability may be poor. Also, if A / B exceeds 2, thermal conductivity may be poor. The sum of the area ratios of each filler group in the elastic layer (A+B) is 0.4 to 0.5. By making A+B 0.4 or more, high thermal conductivity of the elastic layer can be expected, and by making A+B 0.5 or less, excessive increase in hardness of the elastic layer can be suppressed.
[0032] Examples of the first filler having a major axis / minor axis ratio of less than 1.5 include the following commercially available products: alumina such as "Alnabeads CB" (trade name, manufactured by Showa Denko K.K.), zinc oxide such as "LPZINC" (trade name, manufactured by Sakai Chemical Industry Co., Ltd.), magnesium oxide such as "SL-WR" (trade name, manufactured by Konoshima Chemical Co., Ltd.), and silicon oxide (silica) such as "Tospearl" (trade name, manufactured by Momentive Performance Materials, Inc.). Examples of the second filler having a major axis / minor axis ratio of 1.5 or more include the following. The alumina is "LS-130" (product name, manufactured by Nippon Light Metal Co., Ltd.), the zinc oxide is "Panatetra WZ-05F1" (product name, manufactured by Amtec Co., Ltd.), the magnesium oxide is "RF-10C-FC" (product name, manufactured by Ube Materials Corporation), and the silicon oxide (silica) is "S6-5" (product name, manufactured by Marutosha Co., Ltd.). That is, the filler containing an inorganic oxide according to the present disclosure is preferably at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, and silicon oxide.
[0033] The shape of the filler powder may be adjusted by a known spheroidizing process (mechanical spheroidizing process or a spheroidizing method involving melting in a high-temperature atmosphere) or a pulverizing process. The area ratio of the filler measured in the first cross section and the second cross section of the elastic layer corresponds to the volume ratio of the filler in the elastic layer, and can be adjusted by adjusting the volumetric blending ratio of the first filler having a major axis / minor axis ratio of less than 1.5 and the second filler having a major axis / minor axis ratio of 1.5 or more. However, when the strict shape distribution is unknown, the area ratio is finally calculated by image processing described later.
[0034] The elastic layer containing silicone rubber can be formed, for example, by curing an addition-curing liquid silicone rubber composition (unvulcanized rubber composition) containing an addition-curing liquid silicone rubber (unvulcanized rubber) and a filler. The addition-curing liquid silicone rubber can contain (a) an organopolysiloxane having an unsaturated aliphatic group, (b) an organopolysiloxane having active hydrogen bonded to silicon, (c) a catalyst (e.g., a platinum compound), and (d) a cure retarder. (a) functions as a crosslinking point during the curing reaction. (b) is a crosslinking agent. (c) is a catalyst to accelerate the curing reaction. (d) is an inhibitor (curing retarder) to control the reaction start time. In addition to these, fillers suited to the respective purposes can be kneaded and dispersed in order to impart heat resistance, reinforcing properties, etc. Below, (a) to (d) will be explained.
[0035] (a) Organopolysiloxane having an unsaturated aliphatic group Any organopolysiloxane having an unsaturated aliphatic group (hereinafter sometimes referred to as component a) can be used as long as it has an unsaturated aliphatic group such as a vinyl group. For example, the following formulas 1 and 2 can be used as component a.
[0036] ·R 1 R 1The intermediate unit represented by SiO and R 1 R 2 one or both intermediate units selected from the group consisting of intermediate units represented by SiO and R 1 R 1 R 2 SiO 1 / 2 and a molecular end represented by the following formula 1.
[0037] [ka]
[0038] ·R 1 R 1 The intermediate unit represented by SiO and R 1 R 2 one or both intermediate units selected from the group consisting of intermediate units represented by SiO and R 1 R 1 R 1 SiO 1 / 2 and a molecular end represented by the following formula 2.
[0039] [ka]
[0040] (In Equation 1 and Equation 2, R 1 each independently represents an unsubstituted hydrocarbon group that does not contain an unsaturated aliphatic group, R 2 each independently represents an unsaturated aliphatic group, and m and n each independently represent an integer of 0 or more.
[0041] In addition, in Equation 1 and Equation 2, R 1 Examples of the unsubstituted hydrocarbon group not containing an unsaturated aliphatic group include a methyl group, an ethyl group, a propyl group, and an aryl group (e.g., a phenyl group). In particular, a methyl group is preferable. In addition, in Equation 1 and Equation 2, R 2Examples of the unsaturated aliphatic group represented by the formula (I) include a vinyl group, an allyl group, and a 3-butenyl group, with a vinyl group being preferred.
[0042] In formula 1, linear organosiloxanes with n=0 have unsaturated aliphatic groups only at both ends, while linear organosiloxanes with n=1 or more have unsaturated aliphatic groups at both ends and in the side chain. The linear organosiloxanes of formula 2 have unsaturated aliphatic groups only in the side chain. The component a may be used alone or in combination of two or more.
[0043] In addition, when component (a) is used in the elastic layer of the fixing member, the viscosity is set to 100 mm from the viewpoint of excellent moldability. 2 / s or more, 50000mm 2 / s or less. The viscosity (kinetic viscosity) can be measured using a capillary viscometer, a rotational viscometer, or the like based on JIS Z 8803:2011. When using a commercially available component a, the catalog value can be referred to.
[0044] (b) Organopolysiloxane having active hydrogen bonded to silicon (crosslinking agent) Organopolysiloxane having active hydrogen bonded to silicon (hereinafter sometimes referred to as component B) is a crosslinking agent that forms a crosslinked structure by reacting with the unsaturated aliphatic groups in component A through the catalytic action of a platinum compound. Any organopolysiloxane having a Si-H bond can be used as component b, but for example, one that satisfies the following conditions can be suitably used. Note that component b may be used alone or in combination of two or more types.
[0045] From the viewpoint of promoting the formation of a crosslinked structure by reaction with an organopolysiloxane having an unsaturated aliphatic group, the number of hydrogen atoms bonded to silicon atoms is an average of 3 or more per molecule. The organic group bonded to the silicon atom can be, for example, an unsubstituted hydrocarbon group as described above, but a methyl group is preferable. The siloxane skeleton (-Si-O-Si-) may be linear, branched or cyclic. · The Si-H bond may be present in any siloxane unit in the molecule. For example, the linear organopolysiloxanes shown in the following formulas 3 and 4 can be used as component b.
[0046] [ka]
[0047] [ka]
[0048] (In Equation 3 and Equation 4, R 1 each independently represents an unsubstituted hydrocarbon group not containing an unsaturated aliphatic group, p represents an integer of 0 or more, and q represents an integer of 1 or more. In addition, R 1 As explained in Formula 1 and Formula 2, is an unsubstituted hydrocarbon group that does not contain unsaturated aliphatic groups, but is preferably a methyl group.
[0049] (c) Catalyst As the hydrosilylation (addition curing) catalyst, for example, a platinum compound can be used. Specific examples include platinum carbonylcyclovinylmethylsiloxane complex, 1,3-divinyltetramethyldisiloxane platinum complex, etc. Hereinafter, this may be referred to as component c.
[0050] (d) Hardening retarder In order to adjust the curing reaction speed of hydrosilylation (addition curing), a curing retarder can be added. Specific examples include 2-methyl-3-butyn-2-ol and 1-ethynyl-1-cyclohexanol. Hereinafter, this is sometimes referred to as component d.
[0051] The elastic modulus of the elastic layer containing silicone rubber can be adjusted to some extent by the type and amount of the (a) component, the type and amount of the (b) component, the type and amount of the (c) component, and the type and amount of the (d) component. It is more preferable that the elastic layer containing silicone rubber has a (tensile) elastic modulus of 0.20 MPa or more and 1.20 MPa or less. If the elastic modulus of the elastic layer is within this range, the elastic layer has low hardness (flexibility), and a high-quality image can be obtained. In addition, by making it 0.2 MPa or more, it is possible to prevent the elastic layer from deforming when the excess addition-curing type silicone rubber adhesive is squeezed out in the manufacturing process of the fixing member described later.
[0052] The composition of the silicone rubber contained in the elastic layer can be confirmed by performing attenuated total reflection (ATR) measurement using an infrared spectrometer (FT-IR) (for example, product name: Frontier FT IR, manufactured by PerkinElmer). The silicon-oxygen bond (Si-O), which is the main chain structure of silicone, has a wave number of 1020 cm due to stretching vibration. -1 In addition, the methyl group bonded to the silicon atom (Si-CH 3 ) is a bending vibration caused by its structure, and has a wave number of 1260 cm -1 Its presence can be confirmed by the strong infrared absorption in the vicinity.
[0053] The content of the cured silicone rubber and filler in the elastic layer can be confirmed by using a thermogravimetric analyzer (TGA) (for example, product name: TGA851, manufactured by Mettler-Toledo). The elastic layer is cut out with a razor or the like, and about 20 mg is accurately weighed and placed in an alumina pan used in the device. The alumina pan containing the sample is set in the device and heated from room temperature to 800°C at a rate of 20°C per minute in a nitrogen atmosphere, and then kept at 800°C for one hour. In a nitrogen atmosphere, as the temperature rises, the cured silicone rubber component is decomposed and removed by cracking without being oxidized, so the mass of the sample decreases. By comparing the mass before and after the measurement, the content of the cured silicone rubber component and the content of the filler contained in the elastic layer can be confirmed.
[0054] (3-2) Step of applying an electric field to the elastic layer Hereinafter, a corona charger and a process for applying an electric field to an elastic layer using the corona charger will be described as an embodiment. Corona charging methods include a scorotron method having a grid electrode between the corona wire and the body to be charged, and a corotron method not having a grid electrode. The scorotron method is preferred from the viewpoint of excellent controllability of the surface potential of the body to be charged.
[0055] 5(a) and 5(b), the corona charger 2 includes a front block 201, a rear block 202, and shields 203 and 204. A discharge wire 205 is stretched between the front block 201 and the rear block 202. When a charging bias is applied from a high-voltage power supply, the discharge wire 205 discharges and charges the surface of the uncured elastic layer 4 on the substrate as the body to be charged.
[0056] Similar to the configuration of a general corona charger, a high voltage is applied to a discharge wire 205 serving as a discharge member. An ion flow obtained by discharge to the shields 203 and 204 is controlled by applying a high voltage to the grid 206, and the surface potential of the elastic layer 4 is controlled to a desired potential. At this time, since the base 3 or the core 1 holding the base 3 is grounded (not shown), it is possible to generate a desired electric field in the elastic layer 4 by controlling the surface potential of the surface of the elastic layer 4.
[0057] The manufacturing method of the fixing member of the embodiment will be described in detail. First, a layer of an addition curing type liquid silicone rubber composition (hereinafter, also referred to as a "composition layer") 504 containing a first filler and a second filler is formed on a substrate 3. Next, as shown in FIG. 5(a), a corona charger 2 is arranged to face the composition layer 504 in close proximity along the width direction. Then, a voltage is applied to the grid 206 of the corona charger 2, and the substrate 3 is rotated at, for example, 100 rpm for 20 seconds while the corona charger is being discharged. In this way, the surface of the composition layer 504 is charged. The distance between the surface of the composition layer 504 and the grid 206 can be 1 mm to 10 mm. By charging the surface of the composition layer 504 in this way, an electric field is generated in the composition layer 504, and especially the second filler having a major axis / minor axis ratio of 1.5 or more is dielectrically polarized. As a result, the second filler receives a torque and is oriented in the thickness direction of the composition layer 504. Thereafter, the composition layer 504 is cured to obtain the elastic layer 4 in which the orientation of the second filler is fixed.
[0058] From the viewpoint of generating effective electrostatic interaction in the second filler, the voltage applied to the grid 206 is preferably in the range of 0.3 kV to 3 kV in absolute value. When forming the orientation of the irregular filler in the thickness direction of the composition layer 504 using an electric field, it is important to generate an electric field in the thickness direction of the composition layer 504. If the sign of the voltage applied to the grid is the same as the sign of the voltage applied to the wire, the direction of the electric field will be reversed whether it is negative or positive, but the effect obtained will be the same. Depending on the type of thermally conductive filler, it may be difficult to form the orientation of the amorphous filler, and in this case, it is preferable to increase the voltage applied to the grid 206. This is presumed to be related to the dielectric constant of the silicone rubber component and the thermally conductive filler. When the dielectric constant difference between the silicone rubber and the filler is large, it is possible to orient the second filler with a relatively small applied voltage. On the other hand, if the voltage applied to the grid 206 is too large, the electrostatic repulsive force due to the surface charge of the composition layer 504 becomes large, causing the liquid surface to flow, and the surface property of the composition layer 504 may be reduced. Therefore, the voltage applied to the grid 206 is more preferably in the range of 0.6 kV to 2 kV as an absolute value.
[0059] The range of potential control in the longitudinal direction of the surface of the composition 504 is preferably wider than the paper passage area of the fixing member. For example, the configuration shown in FIG. 5(a) can be used, and while a voltage is applied to the grid 206, the composition 504 can be entirely charged by rotating the central axis of the core 1 as the rotation axis. The rotation speed of the fixing belt is preferably 10 rpm to 500 rpm, and the treatment time is preferably 5 seconds or more from the viewpoint of stably orienting the second filler. In this way, the surface potential of the composition layer 504 can be controlled to control the degree of orientation of the second filler.
[0060] Although stainless steel, nickel, molybdenum, tungsten, etc. may be used as the discharge wire 205, it is preferable to use tungsten, which is a very stable metal. The discharge wire stretched inside the shield may have a circular cross section or a sawtooth cross section.
[0061] Moreover, the diameter of the discharge wire 205 is preferably 40 μm to 100 μm. By setting the diameter of the discharge wire within this range, it is possible to suppress cutting of the discharge wire by ions during discharge, and it is also not necessary to make the voltage required to generate a corona discharge excessively high. Either a DC voltage or an AC voltage can be used as the voltage applied to the discharge wire 205. In the case of an AC voltage, it is preferable to apply the voltage at a frequency of about 1 Hz to 1000 Hz. A voltage having a waveform such as a square wave or a sine wave can be output by an arbitrary waveform generator.
[0062] (3-3) Average orientation angle θ of filler in elastic layer Ave How to check The average orientation angle θ of the second filler in the elastic layer Ave This can be confirmed by performing image analysis using a binary image obtained from a cross-sectional image of the elastic layer. As a preliminary step, a cross section for measurement is formed. As shown in FIG. 6, it is preferable to obtain five cross-sectional sample pieces from the first cross-section 4A in the thickness direction-circumferential direction (also referred to as "thickness-circumferential direction") of the elastic layer 4 and five cross-section samples from the second cross-section 4B in the thickness direction-axial direction (also referred to as "thickness-axial direction") in advance using a sharp knife, scissors, or the like. Then, it is preferable to use a cross-section forming method using an ion beam. By using the cross-section forming method using an ion beam, it is possible to prevent the drop-off of filler and the inclusion of unnecessary components such as abrasives, which are likely to occur in cross-section polishing processing, and it is also possible to form a cross-section with few polishing marks. For example, a cross-section polisher can be used for cross-section forming processing using an ion beam.
[0063] Next, the cross section obtained is observed using a laser microscope or a scanning electron microscope (SEM), and a cross-sectional image of a 150 μm × 100 μm area is obtained (Figure 7(a)). The obtained image is converted to black and white using commercially available image software so that the filler part is white and the silicone rubber part is black (Figure 7(b)). As a binarization method, for example, the Otsu method can be used.
[0064] Elliptical approximation is performed on each of the fillers 7A and 7B in the obtained binarized image to obtain a first image (FIG. 7(c)) in which only the fillers 7A with a major axis / minor axis ratio of less than 1.5 remain, and a second image (FIG. 7(d)) in which only the fillers 7B with a major axis / minor axis ratio of 1.5 or more remain. Note that FIG. 7(d) shows an image before elliptical approximation of the fillers 7B whose major axis / minor axis ratio is 1.5 or more when elliptical approximation is performed. Then, from each of the first and second images, A / B is calculated, where A is the area ratio of the first filler 7A whose major axis / minor axis is less than 1.5, and B is the area ratio of the second filler 7B whose major axis / minor axis is 1.5 or more.
[0065] Further, the orientation angle of each filler is calculated by image analysis from a filler image (FIG. 7(d)) that leaves only fillers with a major axis / minor axis ratio of 1.5 or more when elliptical approximation is performed. The orientation angle θ indicates the angle formed when the circumferential direction is 0° (thickness direction is 90°) in the first cross section 4A in the thickness-circumferential direction of the elastic layer, and the axial direction is 0° in the second cross section 4B in the thickness-axial direction. Specifically, if the angle from 0° to the major axis is 90° or less, the angle is defined as the orientation angle θ (FIG. 7(e2)), and if the angle from 0° to the major axis is more than 90°, the angle from the major axis to 180° is defined as the orientation angle θ (FIG. 7(e4)). In this way, the orientation angle θ is defined in the range of 0 to 90° (FIGS. 7(e2) and (e4)). Therefore, the closer the orientation angle is to 90°, the more the filler is oriented in the thickness direction.
[0066] The area ratio of the filler is the average value of the area ratio of the filler at five locations on each of the first cross section 4A in the thickness-circumferential direction of the elastic layer and the second cross section 4B in the thickness-axial direction, totaling ten locations. AveSimilarly, the average value of the orientation angle θ at five locations on each of the first cross section 4A in the thickness-circumferential direction of the elastic layer and the second cross section 4B in the thickness-axial direction, totaling ten locations. The area ratio of the filler is synonymous with the volumetric blending ratio of the filler. Therefore, by adjusting the blending ratio of the spherical filler and the amorphous filler, it is possible to adjust the volumetric blending ratio (area ratio) of the filler with a major axis / minor axis ratio of less than 1.5 and the filler with a major axis / minor axis ratio of 1.5 or more. However, when the exact shape distribution is unknown, the area ratio is finally calculated by image processing.
[0067] The area ratio (A / B) of each filler in the elastic layer is set to be 1 or more and 2 or less. If the area ratio (A / B) is less than 1, durability may be poor. Also, if the area ratio (A / B) is more than 2, thermal conductivity may be poor.
[0068] The sum of the area ratios of each filler in the elastic layer (A+B) is between 0.4 and 0.5. By making the sum of the area ratios (A+B) 0.4 or more, high thermal conductivity of the elastic layer can be expected, and by making the sum of the area ratios (A+B) 0.5 or less, low hardness of the elastic layer can be ensured.
[0069] Average orientation angle θ of filler with major axis / minor axis of 1.5 or more Ave The average orientation angle θ is 50° or more and 90° or less. Since the 90° direction is the thickness direction of the elastic layer, Ave However, the closer the angle is to 90°, the more the filler is oriented in the thickness direction. Ave By setting the angle to be 50° or more and 90° or less, the thermal conductivity in the thickness direction can be increased.
[0070] The thermal conductivity λ of the elastic layer in the thickness direction can be calculated from the following formula. λ=α×C p ×ρ Here, λ is the thermal conductivity of the elastic layer in the thickness direction (W / (m K)), and α is the thermal diffusivity in the thickness direction (m 2 / s), C p is the specific heat at constant pressure (J / (kg K)), and ρ is the density (kg / m 3 ). The method for measuring each parameter will be described in detail in the Examples.
[0071] Furthermore, the flexibility of the elastic layer can be evaluated based on its hardness or tensile modulus. The hardness can be measured, for example, based on Japanese Industrial Standards (JIS) K7312, or using a micro rubber hardness meter (MD-1 TYPE-C hardness meter, manufactured by Kobunshi Keiki Co., Ltd.). The tensile modulus is measured by cutting a sample piece from the elastic layer using a punch (dumbbell-shaped No. 8 type as specified in JIS K6251:2004) and measuring the thickness at the measurement point. Next, the cut sample piece is pulled at a tensile speed of 200 mm / min at room temperature using, for example, a tensile tester (apparatus name: Strograph EII-L1, manufactured by Toyo Seiki Seisakusho Co., Ltd.) to measure the tensile stress. The tensile modulus is measured by creating a graph from the measurement results with the strain of the sample piece on the horizontal axis and the tensile stress on the vertical axis, and the slope of the linear approximation of the measurement data in the strain range of 0 to 10% is used.
[0072] A thermal conductivity of 1.30 W / (m K) or more in the thickness direction of the elastic layer ensures good fixing. A thermal conductivity of 2.00 W / (m K) or more may increase the hardness, so a value of less than 2.00 W / (m K) is preferable.
[0073] (4) Adhesive layer of fixing member The adhesive layer 5 shown in FIG. 4 is an adhesive layer for bonding the elastic layer 4 and the surface layer (release layer) 6. As the adhesive, an adhesive containing an addition-curing liquid silicone rubber mixture containing a self-adhesive component can be suitably used. Specifically, it contains an organopolysiloxane having a plurality of unsaturated aliphatic groups, typically vinyl groups, in the molecular chain, a hydrogenorganopolysiloxane, and a platinum compound as a crosslinking catalyst. It is cured by an addition reaction. As such an adhesive, a known one can be used. Examples of self-adhesive components include:
[0074] Silanes having at least one, preferably two or more, functional groups selected from the group consisting of alkenyl groups such as vinyl groups, acryloxy groups, methacryloxy groups, hydrosilyl groups (SiH groups), epoxy groups, alkoxysilyl groups, carbonyl groups, and phenyl groups; Organosilicon compounds such as cyclic or linear siloxanes having 2 to 30 silicon atoms, preferably 4 to 20 silicon atoms; A non-silicon-based (i.e., silicon-free) organic compound that may contain an oxygen atom in the molecule. The organic compound preferably contains aromatic rings such as phenylene structures having a valence of 1 to 4, more preferably valence of 2 to 4, in one molecule. The organic compound also contains at least one, preferably 2 to 4, functional groups (e.g., alkenyl, acryloxy, methacryloxy groups) that can contribute to a hydrosilylation addition reaction in one molecule.
[0075] The above-mentioned self-adhesive components can be used alone or in combination of two or more. In order to adjust the viscosity or ensure heat resistance, a filler component can be added to the adhesive within the scope of the present disclosure. Examples of the filler component include the following.
[0076] Silica, alumina, iron oxide, titanium oxide, cerium oxide, cerium hydroxide, carbon black, etc. Such addition curing type silicone rubber adhesives are commercially available and are easily available. The thickness of the adhesive layer is preferably 20 μm or less. By setting the thickness to 20 μm or less, the thermal resistance of the fixing member can be set small, and heat from the inner surface side (substrate side) can be efficiently transferred to unfixed toner and recording media such as paper.
[0077] (5) Surface layer of fixing material The surface layer 6 is made of a fluororesin, and a tube method or a coating method is used as a molding method. The following describes the tube method, in which a resin exemplified below is molded into a tube shape and coated. Tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), etc. Among the resin materials listed above, PFA is preferred from the viewpoint of excellent moldability and toner releasability.
[0078] The thickness of the fluororesin layer (surface layer) is preferably 10 μm or more and 50 μm or less, because when the fluororesin layer is laminated on the elastic layer, the elasticity of the underlying elastic layer is maintained, and the surface hardness as a fixing member is prevented from becoming too high, while ensuring abrasion resistance. The inner surface of the fluororesin tube can be preliminarily treated with sodium, excimer laser, ammonia, or the like to improve the adhesiveness.
[0079] 8 is a schematic diagram for explaining an example of a process for laminating a surface layer 6 via an addition-curing silicone rubber adhesive on an elastic layer 4 containing silicone rubber. An addition-curing silicone rubber adhesive is applied to the surface of the elastic layer 4 formed on the outer circumferential surface of a substrate 3. Furthermore, a fluororesin tube 6 as the surface layer 6 is coated on the outer surface of the adhesive and laminated. The method for covering the fluororesin tube is not particularly limited, but may be a method of covering with an addition-curing silicone rubber adhesive as a lubricant, or a method of expanding and covering the fluororesin tube from the outside.
[0080] The excess addition-curing silicone rubber adhesive remaining between the elastic layer 4 and the surface layer 6 made of fluororesin is removed by squeezing it out using a means not shown. The thickness of the adhesive layer 5 after being squeezed out is preferably 20 μm or less from the viewpoint of suppressing a decrease in heat conductivity. Next, the addition-curing silicone rubber adhesive is cured and adhered by heating for a predetermined time with a heating means such as an electric furnace, and both ends in the width direction are cut to the desired length to obtain a fixing member.
[0081] (6) Heat fixing device The thermal fixing device according to the present embodiment is configured so that a pair of heated rollers, belts, or other rotating bodies are pressed against each other. The type of thermal fixing device is appropriately selected in consideration of the overall process speed, size, and other conditions of the image forming apparatus in which the thermal fixing device is mounted. In a thermal fixing device, a fixing nip N is formed by pressing a heated fixing member and a pressure member, and a recording medium S, which is a heated body and has an image formed with unfixed toner, is sandwiched and conveyed through this fixing nip N. The image formed with the unfixed toner is called a toner image t. In this way, the toner image t is heated and pressurized. As a result, the toner image t is melted and mixed, and then cooled to fix the image on the recording medium.
[0082] (7) Image forming device The image forming apparatus according to the present embodiment includes: A photoconductor; a charging device for charging the photoconductor; an exposure device that exposes a charged photoconductor to light to form an electrostatic latent image; a developing device for developing the electrostatic latent image formed on the photoconductor with toner to form a toner image; a transfer device that transfers the toner image formed on the photoreceptor onto a recording medium; The thermal fixing device is also provided.
[0083] A specific example of the thermal fixing device will be given below to explain its configuration, but the scope and applications of the present disclosure are not limited to this example.
[0084] (6-1) Fixing belt-pressure belt type heat fixing device FIG. 9 is a schematic cross-sectional view of an example of a thermal fixing device having a fixing belt as a fixing member, which is a so-called twin-belt type thermal fixing device in which a pair of rotating bodies, namely a fixing belt 11 and a pressure belt 12, are in pressure contact with each other.
[0085] It should be noted that the width direction of the thermal fixing device or the components that make it up is the direction perpendicular to the plane of the paper in Figure 9. The front of the thermal fixing device is the side where the recording medium S is introduced (the right side of Figure 9). The left or right of the thermal fixing device is the left or right when viewed from the front of the thermal fixing device. The belt width is the dimension of the belt in the left-right direction when viewed from the front of the thermal fixing device. The width of the recording medium S is the dimension of the recording medium in a direction perpendicular to the transport direction. Additionally, upstream or downstream is the upstream (right side of Figure 9) or downstream (left side of Figure 9) in relation to the transport direction of the recording medium.
[0086] This thermal fixing device includes fixing members, a fixing belt 11 and a pressure belt 12. The fixing belt 11 and the pressure belt 12 are belts including a flexible base made of a metal whose main component is nickel, as shown in Fig. 4(a), stretched over two rollers.
[0087] As a heating means for heating the fixing belt 11, a heating source (induction heating member, excitation coil) capable of heating by electromagnetic induction heating with high energy efficiency is adopted. The induction heating member 13 is composed of an induction coil 13a, an excitation core 13b, and a coil holder 13c that holds them. The induction coil 13a uses a Litz wire wound flat in an oval shape, and is placed inside a horizontal E-shaped excitation core 13b that protrudes from the center and both sides of the induction coil. The excitation core 13b uses a material with high magnetic permeability and low residual magnetic velocity density such as ferrite or permalloy, so that loss due to the induction coil 13a and excitation core 13b can be suppressed, and the fixing belt 11 can be heated efficiently.
[0088] When a high-frequency current is applied from the excitation circuit 14 to the induction coil 13a of the induction heating member 13, the base of the fixing belt 11 is inductively heated, and the fixing belt 11 is heated from the base side. The surface temperature of the fixing belt 11 is detected by a temperature detection element 15 such as a thermistor. A signal related to the temperature of the fixing belt 11 detected by the temperature detection element 15 is sent to a control circuit unit 16. Based on the temperature information from the temperature detection element 15, the control circuit unit 16 controls the power supplied from the excitation circuit 14 to the induction coil 13a so that the temperature of the fixing belt 11 is maintained at a predetermined temperature.
[0089] The fixing belt 11 is stretched around a roller 17 as a belt rotating member and a heating side roller 18. The roller 17 and the heating side roller 18 are supported by bearings between left and right side plates (not shown) of the device so as to be freely rotatable.
[0090] Roller 17 is, for example, a hollow iron roller having an outer diameter of 20 mm, an inner diameter of 18 mm, and a thickness of 1 mm, and functions as a tension roller that applies tension to fixing belt 11. Heating side roller 18 is, for example, a highly slidable elastic roller having an outer diameter of 20 mm, an inner diameter of 18 mm, a 1 mm thick iron alloy core metal, and a silicone rubber layer as an elastic layer.
[0091] This heating side roller 18, as a drive roller, receives a driving force from a driving source (motor) M via a drive gear train (not shown), and is driven to rotate at a predetermined speed in the clockwise direction indicated by the arrow. By providing the heating side roller 18 with an elastic layer as described above, the driving force input to the heating side roller 18 can be effectively transmitted to the fixing belt 11, and a fixing nip can be formed to ensure separation of the recording medium from the fixing belt 11. By providing the heating side roller 18 with an elastic layer, heat conduction to the heating side roller is also reduced, which is also effective in shortening the warm-up time.
[0092] When the heating side roller 18 is driven to rotate, the fixing belt 11 rotates together with the roller 17 due to frictional force generated between the silicone rubber surface of the heating side roller 18 and the inner surface of the fixing belt 11. The arrangement and size of the roller 17 and the heating side roller 18 are selected according to the size of the fixing belt 11. For example, the dimensions of the roller 17 and the heating side roller 18 are selected so that the fixing belt 11, which has an inner diameter of 55 mm when not installed, can be stretched over them.
[0093] The pressure belt 12 is tensioned by a tension roller 19 and a pressure side roller 20, which serve as belt rotation members. The inner diameter of the pressure belt when not attached is, for example, 55 mm. The tension roller 19 and the pressure side roller 20 are supported by bearings that are freely rotatable between left and right side plates (not shown) of the device.
[0094] The tension roller 19 is, for example, an iron alloy core having an outer diameter of 20 mm, an inner diameter of 16 mm, and a thickness of 2 mm, and is provided with a silicone sponge layer to reduce thermal conductivity and thereby reduce heat conduction from the pressure belt 12. The pressure side roller 20 is, for example, a low-sliding rigid roller made of an iron alloy having an outer diameter of 20 mm, an inner diameter of 16 mm, and a thickness of 2 mm. The dimensions of the tension roller 19 and the pressure side roller 20 are also selected according to the dimensions of the pressure belt 12. Here, in order to form a nip portion N between the fixing belt 11 and the pressure belt 12, the pressure side roller 20 is pressed toward the heating side roller 18 with a predetermined pressure force in the direction of arrow F by a pressure mechanism not shown in the figure at both left and right ends of the rotating shaft.
[0095] In addition, a pressure pad is used to obtain a wide nip portion N without increasing the size of the device. That is, a fixing pad 21 is a first pressure pad that presses the fixing belt 11 toward the pressure belt 12, and a pressure pad 22 is a second pressure pad that presses the pressure belt 12 toward the fixing belt 11. The fixing pad 21 and the pressure pad 22 are supported and disposed between left and right side plates (not shown) of the device. The pressure pad 22 is pressed toward the fixing pad 21 with a predetermined pressure force in the direction of arrow G by a pressing mechanism (not shown). The fixing pad 21, which is the first pressure pad, has a sliding sheet (low friction sheet) 23 that contacts the pad base and the belt. The pressure pad 22, which is the second pressure pad, also has a sliding sheet 24 that contacts the pad base and the belt. This is to suppress abrasion at the portion of the pad that rubs against the inner peripheral surface of the belt. By interposing the sliding sheets 23 and 24 between the belt and the pad base, wear on the pad can be suppressed and sliding resistance can be reduced, ensuring good belt running performance and durability. The fixing belt is provided with a non-contact static electricity removing brush (not shown), and the pressure belt is provided with a contact static electricity removing brush (not shown).
[0096] The control circuit unit 16 drives the motor M at least when image formation is being performed. This causes the heating side roller 18 to rotate, and the fixing belt 11 to rotate in the same direction. The pressure belt 12 rotates following the fixing belt 11. Here, in the most downstream portion of the fixing nip, the heating side roller 18 and the pressure side roller 20 sandwich the fixing belt 11 and the pressure belt 12. This makes it possible to suppress slippage of the fixing belt 11. The most downstream portion of the fixing nip is the portion where the pressure distribution (recording medium conveying direction) in the fixing nip is maximum.
[0097] When the fixing belt 11 is heated to a predetermined fixing temperature and maintained at that temperature (hereinafter referred to as temperature control), the recording medium S having the unfixed toner image t is conveyed to the nip portion N between the fixing belt 11 and the pressure belt 12. The recording medium S is introduced with the surface carrying the unfixed toner image t facing the fixing belt 11. Then, the unfixed toner image t of the recording medium S is nipped and conveyed while being in close contact with the outer peripheral surface of the fixing belt 11, so that heat is applied from the fixing belt 11 and the toner image is fixed on the surface of the recording medium S by applying pressure. At this time, the heat from the heated base of the fixing belt 11 is efficiently transported to the recording medium S through the elastic layer having high thermal conductivity in the thickness direction. After that, the recording medium S is separated from the fixing belt 11 by the separating member 25 and conveyed.
[0098] (6-2) Fixing belt-pressure roller type thermal fixing device 10 is a schematic diagram showing an example of a thermal fixing device of a heating belt-pressure roller type according to one embodiment of the present disclosure, which includes an electrophotographic fixing member having an endless shape, i.e., a fixing belt 11, a pressure roller 33, and a ceramic heater 31, which is a heating body for heating the fixing belt by non-radiant heating, arranged inside the fixing belt 11. Note that, in the thermal fixing device according to the present disclosure, the heater for heating the fixing belt is not limited to the heater for heating the fixing belt by non-radiant heat shown in this embodiment. For example, a heater such as a halogen heater that can heat the fixing belt by radiant heat can also be used. In Fig. 10, the above-mentioned belt is used as the cylindrical or endless fixing belt 11. The fixing belt 11 is held by a heat-resistant and heat-insulating belt guide 30. A ceramic heater 31 for heating the fixing belt 11 is inserted into a groove formed along the guide longitudinal direction (direction perpendicular to the paper surface) at the position where the belt guide 30 contacts the fixing belt 11 (approximately the center of the lower surface of the belt guide 30) and fixedly supported. The fixing belt 11 is loosely fitted around the belt guide 30. A pressure rigid stay 32 is inserted inside the belt guide 30.
[0099] On the other hand, a pressure roller 33 is disposed facing the fixing belt 11. In this embodiment, the pressure roller 33 is an elastic pressure roller, that is, a core metal 33a is provided with an elastic layer 33b of silicone rubber to reduce hardness. The pressure roller 33 is disposed such that both ends of the core metal 33a are rotatably supported by bearings between a chassis side plate (not shown) on the front side of the device and a chassis side plate (not shown) on the rear side. The elastic pressure roller is covered with a PFA (tetrafluoroethylene / perfluoroalkyl ether copolymer) tube (not shown) to improve surface properties.
[0100] Pressure springs (not shown) are respectively compressed between both ends of the pressure rigid stay 32 and spring bearing members (not shown) on the device chassis side, so that a downward force acts on the pressure rigid stay 32. As a result, the lower surface of the ceramic heater 31 disposed on the lower surface of the heat-resistant resin belt guide 30 and the upper surface of the pressure roller 33 are in pressure contact with each other with the fixing belt 11 sandwiched therebetween, forming the fixing nip portion N.
[0101] The pressure roller 33 is driven to rotate in the counterclockwise direction indicated by the arrow by a driving means (not shown). A frictional force acting between the pressure roller 33 and the outer surface of the fixing belt 11 caused by the rotational driving of the pressure roller 33 acts on the fixing belt 11 to rotate it. Then, in the fixing nip portion N, the fixing belt 11 rotates around the outside of the belt guide 30 in the clockwise direction at a peripheral speed substantially corresponding to the rotation peripheral speed of the pressure roller 33 while sliding with its inner peripheral surface in contact with the lower surface of the ceramic heater 31.
[0102] (Pressure roller drive system). The pressure roller 33 starts to rotate based on a print start signal, and the ceramic heater 31 starts to heat up. At the moment when the rotational circumferential speed of the fixing belt 11 due to the rotation of the pressure roller 33 becomes steady and the temperature of the temperature detection element 34 provided on the upper surface of the ceramic heater rises to a predetermined temperature, the recording medium S is introduced into the fixing nip portion N between the fixing belt 11 and the pressure roller 33 and heated. The predetermined temperature is, for example, 180°C. The recording medium S carrying the unfixed toner image t as the heated material is introduced with the toner image carrying surface side facing the fixing belt 11. Then, the recording medium S is in close contact with the lower surface of the ceramic heater 31 via the fixing belt 11 at the fixing nip portion N, and moves and passes through the fixing nip portion N together with the fixing belt 11. During the movement and passing process, the heat of the fixing belt 11 is applied to the recording medium S, and the toner image t is heated and fixed on the surface of the recording medium S. The recording medium S that has passed through the fixing nip portion N is separated from the outer surface of the fixing belt 11 and conveyed.
[0103] The ceramic heater 31 as a heating element is a horizontally elongated linear heating element with low heat capacity, with the longitudinal direction perpendicular to the moving direction of the fixing belt 11 and the recording medium S. The ceramic heater 31 is preferably basically composed of a heater substrate 31a made of aluminum nitride or the like, a heat generation layer 31b provided on the surface of the heater substrate 31a along its longitudinal direction, and a protective layer 31c of glass, fluororesin, or the like provided thereon. The heat generation layer 31b is preferably a layer of an electrical resistance material such as Ag / Pd (silver / palladium) coated by screen printing or the like to a thickness of about 10 μm and a width of 1 to 5 mm. However, the ceramic heater used is not limited to this.
[0104] When electricity is applied between both ends of the heat generating layer 31b of the ceramic heater 31, the heat generating layer 31b generates heat, and the temperature of the heater 31 rises rapidly. The ceramic heater 31 is fixedly supported by being fitted with the protective layer 31c side facing upward into a groove formed along the longitudinal direction of the guide at approximately the center of the lower surface of the belt guide 30. It is preferable that a sliding member 31d is provided on the lower surface of the heater substrate 31a, and that the lower surface of this sliding member 31d and the inner surface of the fixing belt 11 come into contact with each other and slide on each other in the fixing nip portion N that comes into contact with the fixing belt 11.
[0105] As described above, the elastic layer containing silicone rubber has high thermal conductivity in the thickness direction and low hardness in the fixing belt 11. With this configuration, the fixing belt 11 can efficiently heat an unfixed toner image and has low hardness, so that a high-quality image can be fixed onto the recording medium S. As described above, according to one aspect of the present disclosure, there is provided a thermal fixing device including the fixing member as described above, which has excellent fixing performance and can fix a high-quality image. As described above, according to one aspect of the present disclosure, there is provided a fixing member having a low hardness elastic layer that has high thermal conductivity in the thickness direction and is resistant to fracture or plastic deformation even when repeatedly compressed at high temperatures. According to another aspect of the present disclosure, there is provided a thermal fixing device and an image forming apparatus that have excellent fixing properties, can form high-quality electrophotographic images, and are excellent in paper feed durability. EXAMPLES
[0106] The present disclosure will now be described in more detail with reference to examples. [Hardness unevenness comparison test] A comparison was made in terms of hardness unevenness between an elastic layer sample produced using parallel plate electrodes and an elastic layer sample produced using a corona charger according to an embodiment of the present disclosure.
[0107] (1) Preparation of liquid addition-curable silicone rubber composition First, 98.6 parts by mass of silicone rubber having vinyl groups, which are unsaturated aliphatic groups, only at both ends of the molecular chain and methyl groups as unsubstituted hydrocarbon groups containing no other unsaturated aliphatic groups, was prepared as component a. This silicone rubber (trade name: DMS-V35, manufactured by Gelest, viscosity 5,000 mm 2 / s) will be referred to as "Vi" from here on.
[0108] Next, 220 parts by mass of spherical alumina (product name: CB-P10, manufactured by Showa Denko K.K.) was added as a thermally conductive filler to this Vi. Furthermore, 120 parts by mass of amorphous alumina (product name: LS-130, manufactured by Nippon Light Metal Co., Ltd.) was added and thoroughly mixed to obtain mixture 1. Next, 0.2 parts by mass of 1-ethynyl-1-cyclohexanol (manufactured by Tokyo Chemical Industry Co., Ltd.), a cure retarder as component d, was dissolved in the same mass of toluene and added to mixture 1 to obtain mixture 2.
[0109] Next, 0.1 parts by mass of a hydrosilylation catalyst (platinum catalyst: a mixture of 1,3-divinyltetramethyldisiloxane platinum complex, 1,3-divinyltetramethyldisiloxane, and 2-propanol) as component c was added to mixture 2 to obtain mixture 3.
[0110] Furthermore, as component b, a silicone rubber having a linear siloxane skeleton and having active hydrogen groups bonded to silicon only on the side chain (product name: HMS-301, manufactured by Gelest, viscosity 30 mm) was used. 2 1.4 parts by mass of dimethylformamide / s (hereinafter referred to as "SiH") was weighed out. This was added to mixture 3 and mixed thoroughly to obtain a liquid addition-curable silicone rubber composition.
[0111] (2-1) Preparation of parallel plate electrode sample The silicone rubber composition was sandwiched between a 500 μm thick acrylic spacer and an indium tin oxide (hereinafter referred to as "ITO") glass electrode to prepare a sample piece having a thickness of 500 μm and a square shape with a side length of 50 mm. A power source was connected to the ITO glass electrode, and while applying an AC voltage of 950 V and a frequency of 60 Hz, the silicone rubber was cured by leaving it to stand for 2 hours in an environment at a temperature of 80°C. The cured silicone rubber was then peeled off from the electrode and left to stand for 30 minutes in an environment at a temperature of 200°C for secondary curing, yielding a parallel plate electrode sample.
[0112] (2-2) Preparation of corona-charged sample An uncured film of the silicone rubber composition having a thickness of 500 μm was formed on a stainless steel film (hereinafter also referred to as "SUS film") using a slit coater. The SUS film was attached to a cylindrical core and charged with a corona charger while rotating. The conditions were a rotation speed of 100 rpm, a current supplied to the corona charger wire of -150 μA, a grid electrode potential of -950 V, a charging time of 20 seconds, and a distance of 4 mm between the grid electrode and the uncured film. This charged uncured sample was heated in an electric furnace at 160°C for 1 minute (primary curing), and then heated in an electric furnace at 200°C for 30 minutes (secondary curing) to cure the silicone rubber composition, thereby obtaining a corona-charged sample.
[0113] (3) Hardness unevenness evaluation of samples Each of the obtained samples was molded into a square with a side length of 50 mm, and the rubber hardness was measured at 10 points on the surface using a micro rubber hardness meter (MD-1 TYPE-C hardness meter, manufactured by Kobunshi Keiki Co., Ltd.), and the average value and standard deviation of the rubber hardness were calculated. The results were as follows: Corona-charged sample: average rubber hardness 64.1°, standard deviation 1.7° Parallel plate electrode sample: average rubber hardness 65.5°, standard deviation 7.3° The parallel plate electrode sample had large hardness variations, and it was found that it was difficult to apply it to a fixing member.
[0114] [Example 1] (1) Preparation of liquid addition-curable silicone rubber composition In the same manner as in the hardness unevenness comparison test, a liquid addition-curable silicone rubber composition was obtained.
[0115] (2) Preparation of the fixing belt An electroformed nickel endless belt having an inner diameter of 55 mm, a width of 420 mm, and a thickness of 65 μm was prepared as a substrate. During the series of manufacturing steps, the endless belt was handled with a core inserted therein. A primer (product name: DY39-051A / B; manufactured by Dow Corning Toray Co., Ltd.) was applied approximately uniformly to the outer peripheral surface of the substrate so that the dry mass was 50 mg. After the solvent was dried, the substrate was baked for 30 minutes in an electric furnace set to 160°C.
[0116] Onto this primer-treated substrate, the above silicone rubber composition was applied by ring coating to a thickness of 450 μm. This is referred to as an uncured endless belt. Next, a corona charger was placed facing the generator of the uncured endless belt, and the surface of the uncured elastic layer was charged while rotating the uncured endless belt at 100 rpm under the following conditions: current supplied to the discharge wire of the corona charger was -150 μA, grid electrode potential was -950 V, charging time was 20 seconds, and distance between the grid electrode and the belt was 4 mm.
[0117] This charged uncured endless belt was heated in an electric furnace at 160°C for 1 minute (primary curing), and then heated in an electric furnace at 200°C for 30 minutes (secondary curing) to cure the silicone rubber composition, thereby obtaining an endless belt with a cured elastic layer. Next, an addition-curing silicone rubber adhesive (product name: SE1819CV A / B; manufactured by Toray Dow Corning Co., Ltd.) was applied almost uniformly to a thickness of about 20 μm on the surface of the elastic layer of the cured endless belt to form an adhesive layer. Next, a fluororesin tube (product name: NSE; manufactured by Gunze Co., Ltd.) with an inner diameter of 52 mm and a thickness of 40 μm was laminated on the adhesive layer as a release layer while expanding its diameter. After that, the belt surface was uniformly rubbed from above the fluororesin tube to remove excess adhesive from between the elastic layer and the fluororesin tube, so that the thickness of the adhesive layer was thinned to about 5 μm. The endless belt was heated for 1 hour in an electric furnace set at 200° C. to harden the adhesive and fix the fluororesin tube onto the elastic layer. Both ends of the obtained endless belt were cut to obtain a fixing belt with a width of 368 mm.
[0118] (3) Evaluation of characteristics of the elastic layer of the fixing belt (3-1) Evaluation of filler area ratio and orientation in the cross section of the elastic layer in the thickness direction From the elastic layer of the produced fixing belt, 5 locations from the first cross section in the thickness-circumferential direction and 5 locations from the second cross section in the thickness-axial direction, totaling 10 locations, were cut out to a size of 5 mm x 5 mm, and observation cross sections were formed using an ion beam. A cross-section polisher (product name: SM09010; manufactured by JEOL Ltd.) was used for the cross section formation, and the applied voltage was set to 4.5 V in an argon gas atmosphere, and the ion beam was irradiated from the base side in the thickness direction of the fixing belt for 11 hours to prepare the observation cross sections. The reason for irradiating the fixing belt with an ion beam in the thickness direction from the base side is that if irradiation is performed from the surface side, the shavings of the fluororesin of the surface layer will adhere to the surface. The obtained observation cross section was observed with a laser microscope (product name: OLS3000, manufactured by Olympus Corporation) using a 50x objective lens, and a cross-sectional image of 150 μm × 100 μm in size was obtained.
[0119] The cross-sectional images were then binarized using the image processing software ImageJ (manufactured by the National Institutes of Health, USA) using the Otsu method. From the obtained binarized image, it was found that the area ratio A of the first filler particles having a major axis / minor axis ratio of less than 1.5 was 0.30, and the area ratio B of the second filler particles having a major axis / minor axis ratio of 1.5 or more was 0.16. Next, the average orientation angle θ Ave The average orientation angle θ Ave was 60°.
[0120] (3-2) Thermal conductivity of the elastic layer in the thickness direction The thermal conductivity λ of the elastic layer in the thickness direction was calculated from the following formula. λ=α×C p ×ρ In the formula, λ is the thermal conductivity of the elastic layer in the thickness direction (W / (m K)), α is the thermal diffusivity in the thickness direction (m 2 / s), C p is the specific heat at constant pressure (J / (kg K)), and ρ is the density (kg / m 3 ) where the thermal diffusivity α in the thickness direction and the specific heat at constant pressure C p The values of and density ρ were obtained by the following method.
[0121] ·Thermal diffusivity α The thermal diffusivity α in the thickness direction of the elastic layer was measured at room temperature (25°C) using a periodic heating method thermal property measurement device (product name: FTC-1, manufactured by Advance Riko Co., Ltd.). Sample pieces with an area of 8 mm × 12 mm were cut from the elastic layer with a cutter to prepare a total of five sample pieces, and the thickness of each sample piece was measured using a digital length measuring device (product name: DIGIMICRO (registered trademark) MF-501 flat measuring probe φ4 mm; manufactured by Nikon Corporation). Next, a total of five measurements were made for each sample piece, and the average value (m 2 The measurement was performed while applying pressure to the sample using a 1 kg weight. As a result, the thermal diffusivity α of the silicone rubber elastic layer in the thickness direction was 6.33×10 -7 m 2 / s.
[0122] Constant pressure specific heat C P The constant pressure specific heat of the elastic layer was measured using a differential scanning calorimeter (product name: DSC823e, manufactured by Mettler Toledo Co., Ltd.). Specifically, aluminum pans were used as the sample pan and the reference pan. First, as a blank measurement, both pans were empty and kept at a constant temperature of 15°C for 10 minutes, then the temperature was increased to 215°C at a rate of 10°C / min, and the temperature was kept constant at 215°C for another 10 minutes. Next, 10 mg of synthetic sapphire with a known specific heat at constant pressure was used as the reference material, and the same program was used to perform the measurement. Next, a 10 mg measurement sample, the same amount as the synthetic sapphire reference material, was cut out from the elastic layer, set in the sample pan, and measured using the same program. These measurement results were analyzed using the specific heat analysis software attached to the differential scanning calorimeter, and the constant pressure specific heat C at 25°C was calculated from the average of the five measurement results. P was calculated. As a result, the specific heat at constant pressure of the silicone rubber elastic layer was found to be 0.94 J / (g·K).
[0123] ·Density ρ The density of the elastic layer was measured using a dry automatic densitometer (product name: Accupyc 1330-01, manufactured by Shimadzu Corporation). Specifically, 10 cm 3 A sample cell was used, and a sample piece was cut out from the elastic layer so as to fill approximately 80% of the cell volume. The mass of this sample piece was measured and then placed in the sample cell. This sample cell was set in the measurement section of the device, and helium was used as the measurement gas. After gas replacement, the volume measurement was carried out 10 times. The density of the elastic layer was calculated from the mass of the sample piece and the measured volume for each measurement, and the average value was calculated. As a result, the density of the silicone rubber elastic layer was 2.35 g / cm 3 It was.
[0124] Unit converted specific heat of elastic layer at constant pressure C p (J / (kg K)) and density ρ(kg / m 3 ), and the measured thermal diffusivity α(m 2The thermal conductivity λ of the elastic layer in the thickness direction was calculated from the thermal conductivity (Tc) of the elastic layer, and was found to be 1.40 W / (m K).
[0125] (3-3) Tensile modulus of elastic layer In order to confirm that the elastic layer has a low hardness, the tensile modulus of the elastic layer was measured. Specifically, a sample piece was cut out from the elastic layer using a punching die (dumbbell-shaped No. 8 type as specified in JIS K6251:2004), and the thickness near the center, which is the measurement point, was measured. Next, the cut-out sample piece was tested at a tensile speed of 200 mm / min and room temperature using a tensile tester (device name: Strograph EII-L1, manufactured by Toyo Seiki Seisakusho Co., Ltd.). The tensile modulus was determined by creating a graph from the measurement results with the strain of the sample piece on the horizontal axis and the tensile stress on the vertical axis, and the slope of the linear approximation of the measurement data in the strain range of 0 to 10%. As a result, the tensile modulus of the elastic layer was 0.63 MPa.
[0126] (4) Evaluation of high temperature and pressure resistance of the elastic layer of the fixing belt Four sample pieces each having a size of 50 mm×50 mm were cut out from the obtained fixing belt, and each sample piece was supported on a stainless steel plate (SUS plate) 40 (FIG. 11) to form four test pieces. The high-temperature pressure resistance of these four test pieces was evaluated using a jig shown in Fig. 11. In this jig, the surface temperature of the sample (fixing belt 11) was set to a high temperature by a heater 41 and a thermistor 42, and a pressing roller 43 (width 10 mm, diameter 15 mm) was moved back and forth relatively left and right, so that the high-temperature pressure resistance could be evaluated. In this test, the surface temperature of each test piece was set to 240° C., and the pressing roller 43 was moved back and forth relatively to the left and right under a load of 15 N, and the average time until the sample pieces broke or were plastically deformed was calculated. If the sample pieces did not break or plastically deform after 10 hours of testing, the durability was evaluated as good, and the test was terminated. As a result, in this embodiment, the sample pieces did not break or undergo plastic deformation even after 10 hours had elapsed, and the durability was good.
[0127] (5) Actual machine evaluation (fixing ability, image quality, durability) The fixing belt obtained as described above was incorporated into a thermal fixing device of an electrophotographic copying machine (product name: imagePRESS (registered trademark) C850, manufactured by Canon Inc.). Using a copying machine equipped with this thermal fixing device, a fixing test was performed on thick paper. In addition, fixing evaluation, image quality evaluation, and paper feed durability test were performed using plain paper.
[0128] For the adhesion test of thick paper, the basis weight is 300g / m 2 Paper (UPM PAPER, UPM Finesse (registered trademark) gloss 300g / m 2 ) was used. Then, five sheets of blue solid images were printed in succession at a temperature lower than the standard temperature (195° C.), and the fixing property was evaluated based on whether the toner was fixed to the paper. As a result, it was found that the toner was fixed to the paper even when the temperature was controlled to 185°C, 10°C lower than the standard, and that the thermal conductivity of the elastic layer of the fixing belt was extremely excellent.
[0129] The image quality was also evaluated by visual inspection from the viewpoint of whether or not there was uneven gloss on the image. As a result, due to the low hardness and lack of hardness unevenness of the elastic layer, there was no unevenness in gloss and the image quality was extremely excellent. If the elastic layer had a high hardness or had uneven hardness, it would lose its ability to conform to the unevenness of the paper fibers, resulting in uneven gloss, but such uneven gloss did not occur.
[0130] In the paper feed durability test, the paper was printed on 80g / m2 high-quality color laser copier paper. 2 (Canon Inc.) A4 paper was fed continuously in the short direction (80 sheets / min). In addition, coated paper OK top coat 128g / m was applied every 100,000 sheets. 2A uniform cyan halftone image was formed on a 13 x 19 inch paper (manufactured by Oji Paper Co., Ltd.). This image was visually inspected for image defects such as scratches, streaks, uneven gloss, etc. If the number of sheets passed when the image defect was confirmed was less than 600,000, the number of sheets passed when the image defect was confirmed was recorded, and the durability was determined to be poor and the test was terminated. If the number of sheets passed when the image defect was confirmed was more than 600,000, the durability was determined to be good and the test was terminated. In this embodiment, no image defects occurred even after printing more than 600,000 sheets, and therefore it was determined that the durability was good.
[0131] [Examples 2 to 4] The mixing ratio of the spherical alumina and amorphous alumina fillers was adjusted so that the area ratio A of the first filler having a major axis / minor axis ratio of less than 1.5 and the area ratio B of the second filler having a major axis / minor axis ratio of 1.5 or more were set to the values shown in Table 1. Except for this, a fixing belt was produced and evaluated in the same manner as in Example 1.
[0132] [Example 5] The mixing ratio of the spherical alumina and amorphous alumina fillers was adjusted, and spherical silica filler (product name: Tospearl, manufactured by Toshiba Silicones Co., Ltd.) was added. The area ratio A of the first filler (alumina + silica) having a major axis / minor axis ratio of less than 1.5 was set to 0.25, and the area ratio B of the second filler (alumina) having a major axis / minor axis ratio of 1.5 or more was set to 0.17. A fixing belt was produced and evaluated in the same manner as in Example 1 except for the above points.
[0133] [Example 6] As the filler, nearly spherical magnesium oxide (product name: SL-WR, manufactured by Konoshima Chemical Co., Ltd.) and amorphous magnesium oxide (product name: RF-10C-FC, manufactured by Ube Material Industries, Ltd.) were used. The area ratio A of the first filler having a major axis / minor axis ratio of less than 1.5 was set to 0.20, and the area ratio B of the second filler having a major axis / minor axis ratio of 1.5 or more was set to 0.20. A fixing belt was produced and evaluated in the same manner as in Example 1 except for the above points.
[0134] [Example 7] As the filler, nearly spherical zinc oxide (product name: LPZINC-11; manufactured by Sakai Chemical Industry Co., Ltd.) and amorphous zinc oxide (product name: Panatetra WZ-05F1; manufactured by Matsushita Amtec Co., Ltd.) were used. The area ratio A of the first filler particles having a major axis / minor axis ratio of less than 1.5 was set to 0.25, and the area ratio B of the second filler particles having a major axis / minor axis ratio of 1.5 or more was set to 0.20. A fixing belt was produced and evaluated in the same manner as in Example 1 except for the above points.
[0135] [Comparative Example 1] A fixing belt was produced and evaluated in the same manner as in Example 1, except that no electric field was applied.
[0136] [Comparative Example 2] No electric field was applied, and the mixing ratio of the spherical alumina and amorphous alumina fillers was adjusted so that the area ratio A of the first filler having a long axis / short axis ratio of less than 1.5 was 0.30, and the area ratio B of the second filler having a long axis / short axis ratio of 1.5 or more was 0.25. A fixing belt was produced and evaluated in the same manner as in Example 1 except for the above points.
[0137] [Comparative Examples 3 to 5] The mixing ratio of the spherical alumina and amorphous alumina fillers was adjusted so that the area ratio A of the first filler having a major axis / minor axis ratio of less than 1.5 and the area ratio B of the second filler having a major axis / minor axis ratio of 1.5 or more were set to the values shown in Table 1. Except for this, a fixing belt was produced and evaluated in the same manner as in Example 1.
[0138] The results are shown in Tables 1 and 2. The evaluation of the fixing belt's fixing performance and image quality is based on the following criteria. (1) Fixability Rank A: The toner was fixed on the paper at a temperature 15°C lower than the standard temperature (195°C). Rank B: The toner was fixed on the paper at a temperature 10°C lower than the standard temperature (195°C). Rank D: The toner did not fix to the paper when the temperature was controlled 10° C. lower than the standard temperature (195° C.). (2) Image quality Rank A: The gloss was excellent with no unevenness. Rank B: Excellent with no uneven gloss. Rank C: There was some unevenness in gloss. Rank D: There was uneven gloss. - : Image quality not rated
[0139] [Table 1]
[0140] [Table 2]
[0141] The results shown in Tables 1 and 2 reveal the following: In Comparative Example 1 where no electric field was applied, the second filler particles having a major axis / minor axis ratio of 1.5 or more were not oriented (average orientation angle θ Ave is less than 50°). On the other hand, in Example 1 in which an electric field was applied, the second filler particles having a major axis / minor axis ratio of 1.5 or more were oriented in the thickness direction (average orientation angle θ Ave The thermal conductivity in the thickness direction was increased when the angle was between 50° and 90°.
[0142] In addition, when Examples 1 to 7 are compared with Comparative Examples 3 to 5, when 1.0≦(A / B)≦2.0 and 0.40≦(A+B)≦0.50, the second filler particles having a major axis / minor axis ratio of 1.5 or more are oriented in the thickness direction. The thermal conductivity in the thickness direction is also high. As a result, it is found that Examples 1 to 7 have good fixability. Specifically, in all examples, the thermal conductivity in the thickness direction is 1.30 W / (m K) or more, which means good fixability, and those with a thermal conductivity in the thickness direction of 1.60 W / (m K) or more have even better fixability. On the other hand, in Comparative Examples 1, 3, and 5, in which the thermal conductivity in the thickness direction was less than 1.30 W / (m·K), the fixing property was low.
[0143] Also, it is found that the elastic layers of the fixing members according to Examples 1 to 7 have a low tensile modulus of elasticity of 0.20 MPa or more and 1.20 MPa or less (1.20 MPa is about 50° in Asker C hardness (JIS K7312)), and thus have low hardness. As a result, it was found that the fixing members of Examples 1 to 7 can conform to the unevenness of the fibers of the paper, which is the recording medium, in the fixing nip, making it difficult for uneven softening and melting of the toner to occur, and enabling the production of high-quality images. On the other hand, in Comparative Example 2 in which the tensile modulus exceeded 1.20 MPa, high quality images could not be obtained.
[0144] Furthermore, in the evaluation of pressure resistance durability at high temperatures, all examples were 5 hours or more, and most of them showed good durability even after 10 hours or more without breaking or plastic deformation. As a result, high durability was also achieved in the paper feed durability test in which repeated stress was applied at high temperatures. [Explanation of symbols]
[0145] 1 core 2 Corona charger 3 Base 4 Elastic layer 4A 1st section 4B 2nd cross section 5 Adhesive layer 6 Surface layer 7. Filler 7A First filler with major axis / minor axis less than 1.5 7B Second filler with major axis / minor axis of 1.5 or more 11 Fixing belt 12 Pressure Belt 13 Induction heating components 13a Induction coil 13b Excitation core 13c Coil Holder 14 Excitation circuit 15 Temperature detection element 16 Control circuit section 17. Lola 18 Heating roller 19 Tension roller 20 Pressure roller 21 Fixing Pad 22 Pressure Pad 23, 24 Sliding sheet 25 Separation member 30 Belt guide 31 Ceramic heater 31a Heater board 31b Heating layer 31c protective layer 31d Sliding member 32 Stay 33 Pressure roller 33a Core metal 33b Elastic layer 34 Temperature detection element 40 Stainless steel plate 41 Heater 42 Thermistor 43 Pressing roller N Fixing nip t Unfixed toner S Recording medium Medium motor
Claims
1. A substrate; an elastic layer provided on an outer periphery of the substrate, The elastic layer includes a filler including an inorganic oxide, The filler includes at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, and silicon oxide; (1) in a binarized image of a first cross section of the elastic layer in the thickness-circumferential direction and a binarized image of a second cross section of the elastic layer in the thickness-axial direction, When the shape of the filler is approximated as an ellipse, The area ratio of the first filler having a major axis / minor axis ratio of less than 1.5 is A, When the area ratio of the second filler having a major axis / minor axis ratio of 1.5 or more is B, 1.0≦(A / B)≦2.0 and 0.40≦(A+B)≦0.50; (2) The average orientation angle θAve of the second filler having a major axis / minor axis ratio of 1.5 or more with respect to the thickness direction of the elastic layer is 50°≦θAve≦90°. and the first filler is a spherical inorganic oxide, The electrophotographic fixing member according to claim 1, wherein the second filler is an amorphous inorganic oxide.
2. 2. The electrophotographic fixing member according to claim 1, wherein the thermal conductivity in the thickness direction of the elastic layer is 1.30 W / (m·K) or more and less than 2.00 W / (m·K).
3. 3. The electrophotographic fixing member according to claim 1, wherein the spherical inorganic oxide and the amorphous inorganic oxide are both alumina.
4. 4. The electrophotographic fixing member according to claim 1, wherein the elastic layer contains a silicone rubber as a binder.
5. 5. The electrophotographic fixing member according to claim 1, wherein the electrophotographic fixing member is a fixing belt having an endless shape.
6. 6. The electrophotographic fixing member according to claim 5, which is used as a fixing belt of a fixing device which fixes an unfixed toner image on a recording medium using a fixing belt heated by non-radiative heat.
7. A fixing device for fixing an unfixed toner image on a recording medium by heating the unfixed toner image on the recording medium with an electrophotographic fixing member, A fixing device, comprising the electrophotographic fixing member according to any one of claims 1 to 6.
8. The electrophotographic fixing member is a fixing belt according to claim 5 or 6, the fixing device forms a fixing nip together with the fixing belt and a pressure member disposed opposite the fixing belt, 10. The fixing device according to claim 9, wherein a heater for heating the fixing belt with non-radiative heat is in contact with an inner peripheral surface of the fixing belt.
9. A photoconductor; a charging device for charging the photoconductor; an exposure device that exposes a charged photoconductor to light to form an electrostatic latent image; a developing device for developing the electrostatic latent image formed on the photoconductor with toner to form a toner image; a transfer device that transfers the toner image formed on the photoreceptor onto a recording medium; A fixing device; An image forming apparatus having The fixing device heats an unfixed toner image on the recording medium with an electrophotographic fixing member to fix the unfixed toner image on the recording medium. A fixing device for fixing onto a body, The electrophotographic fixing member is the electrophotographic fixing member according to any one of claims 1 to 6.
1. An image forming apparatus comprising:
Citation Information
Patent Citations
Fixing member and fixing device
JP2005300591A
Heat fixing member and heat fixing apparatus
JP2006259712A
Fixing roller, method for manufacturing fixing roller, fixing device, and image forming apparatus
JP2007101736A
Resin composition, and method for producing the same
JP2013159748A
Pressure roller, fixing device, and image forming apparatus
JP2015001692A