Piezoelectric thin film, piezoelectric thin film element, and piezoelectric transducer

A piezoelectric thin film with oriented tetragonal crystals in a perovskite oxide structure addresses the challenge of high dielectric constants in conventional materials, achieving a large piezoelectric figure of merit for improved piezoelectric performance.

JP7588007B2Active Publication Date: 2024-11-21TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021037452
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-09
Publication Date
2024-11-21
Estimated Expiration
2041-03-09

AI Technical Summary

Technical Problem

Conventional piezoelectric materials, such as lead zirconate titanate (PZT), face challenges in achieving a large piezoelectric figure of merit due to high dielectric constants, making them unsuitable for thin film applications, and there is a need for lead-free alternatives with improved piezoelectricity.

Method used

A piezoelectric thin film comprising a first and second piezoelectric layer with oriented tetragonal crystals, where the (001) planes of both layers are aligned normal to the film surface, and the spacing ratio c2/a2 is controlled to enhance piezoelectricity, using perovskite oxides like BiFeO3 with additional elements to stabilize the tetragonal structure.

Benefits of technology

The proposed structure achieves a large piezoelectric figure of merit by optimizing the dielectric constant and piezoelectric constant ratio, resulting in enhanced performance for piezoelectric thin film elements and transducers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588007000010
    Figure 0007588007000010
  • Figure 0007588007000011
    Figure 0007588007000011
  • Figure 0007588007000012
    Figure 0007588007000012
Patent Text Reader

Abstract

To provide a piezoelectric thin film with a large piezoelectric performance index.SOLUTION: A piezoelectric thin film 3 includes a first piezoelectric layer 3A, and a second piezoelectric layer 3B directly overlapping the first piezoelectric layer 3A. The first piezoelectric layer 3A contains a tetragonal crystal 1 of a perovskite type oxide, and the second piezoelectric layer 3B contains a tetragonal crystal 2 of a perovskite type oxide. A (001) plane of the tetragonal crystal 1 is oriented in a normal direction dn of a surface of the piezoelectric thin film 3. A (001) plane of the tetragonal crystal 2 is oriented in the normal direction dn of the surface of the piezoelectric thin film 3. An interval of a (001) plane of a tetragonal crystal 1 is c1, and an interval of a (100) plane of the tetragonal crystal 1 is a1, an interval of a (001) plane of a tetragonal crystal 2 is c2, and an interval of a (100) plane of the tetragonal crystal 2 is a2, c2 / a2 is more than c1 / a1, and c1 / a1 is equal to or more than 1.015 and equal to or less than 1.050.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a piezoelectric thin film, a piezoelectric thin film element, and a piezoelectric transducer. [Background technology]

[0002] Piezoelectric materials are processed into various piezoelectric elements for various purposes. For example, a piezoelectric actuator converts voltage into force by applying a voltage to a piezoelectric material, which deforms the material, through the inverse piezoelectric effect. A piezoelectric sensor also converts force into voltage by applying pressure to a piezoelectric material, which deforms the material, through the piezoelectric effect. These piezoelectric elements are installed in various electronic devices.

[0003] In recent years, in response to market demands for miniaturization and improved performance of electronic devices, there has been active research into piezoelectric elements (piezoelectric thin film elements) that use piezoelectric thin films. However, the thinner the piezoelectric body is, the more difficult it is to obtain the piezoelectric effect and inverse piezoelectric effect, so there is a demand for the development of piezoelectric bodies that have excellent piezoelectric properties in a thin film state.

[0004] Conventionally, lead zirconate titanate (PZT), a perovskite-type ferroelectric, has been widely used as a piezoelectric material. However, since PZT contains lead (Pb), which is harmful to the human body and the environment, the development of lead-free piezoelectric materials as an alternative to PZT is expected. For example, the following Non-Patent Document 1 describes BiFeO3 as an example of a lead-free piezoelectric material. Among lead-free piezoelectric materials, BiFeO3 has relatively excellent piezoelectric properties, and is particularly expected to be applied to piezoelectric thin film elements. The following Patent Document 1 describes a piezoelectric material made of Bi(Co,Fe)O3 and containing a mixture of tetragonal crystals and rhombohedral crystals as a piezoelectric material with better piezoelectric properties than conventional BiFeO3. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-191870 A [Non-patent literature]

[0006] [Non-Patent Document 1] K.Ujimoto et al, Direct piezoelectric properties of (100) and (111) BiFeO3 epitaxial thin films, APPLIED PHYSICS LETTERS. 100, 102901 (2012) Summary of the Invention [Problem to be solved by the invention]

[0007] (-e 31,f ) 2 / ε0ε r is the piezoelectric performance index that indicates the piezoelectricity of the piezoelectric thin film. -e 31,f is a type of piezoelectric constant, -e 31,f The unit is C / m 2 ε0 is the dielectric constant of a vacuum, and the unit of ε0 is F / m. ε r is the relative dielectric constant of the piezoelectric thin film, and ε r There is no unit. (-e 31,f ) 2 / ε0ε r The unit of is Pa. A piezoelectric thin film having a large piezoelectric figure of merit is suitable for piezoelectric thin film elements such as piezoelectric transducers (sensors). However, conventional piezoelectric materials that are a mixture of tetragonal and rhombohedral crystals have excellent piezoelectric properties, but because they have a relatively high relative dielectric constant, they do not have a sufficiently large piezoelectric figure of merit. Therefore, conventional piezoelectric materials are not fully suitable for piezoelectric thin film elements such as piezoelectric transducers (sensors).

[0008] An object of one aspect of the present invention is to provide a piezoelectric thin film having a large piezoelectric figure of merit, and a piezoelectric thin film element and a piezoelectric transducer including the piezoelectric thin film. [Means for solving the problem]

[0009] A piezoelectric thin film according to one aspect of the present invention is a piezoelectric thin film comprising a first piezoelectric layer and a second piezoelectric layer directly overlapping the first piezoelectric layer, the first piezoelectric layer including a tetragonal crystal 1 of a perovskite type oxide, the second piezoelectric layer including a tetragonal crystal 2 of a perovskite type oxide, the (001) plane of the tetragonal crystal 1 being oriented in a normal direction to a surface of the piezoelectric thin film, the (001) plane of the tetragonal crystal 2 being oriented in a normal direction to a surface of the piezoelectric thin film, the spacing between the (001) planes of the tetragonal crystal 1 being c1, the spacing between the (100) planes of the tetragonal crystal 1 being a1, the spacing between the (001) planes of the tetragonal crystal 2 being c2, the spacing between the (100) planes of the tetragonal crystal 2 being a2, c2 / a2 being greater than c1 / a1, and c1 / a1 being 1.015 or greater and 1.050 or less.

[0010] c2 / a2 may be greater than or equal to 1.051 and less than or equal to 1.250.

[0011] The peak intensity of the diffracted X-rays from the (001) plane of the tetragonal crystal 1 is I1, the peak intensity of the diffracted X-rays from the (001) plane of the tetragonal crystal 2 is I2, and I2 / (I1+I2) may be 0.90 or more and less than 1.00.

[0012] Perovskite oxide is composed of bismuth, iron, and element E. B and oxygen, element E B may be at least one element selected from the group consisting of magnesium, aluminum, zirconium, titanium, nickel and zinc.

[0013] The tetragonal crystal 1 may be represented by the following chemical formula 1, and E in the following chemical formula 1 A may be at least one element selected from the group consisting of Na, K and Ag, and E in the following chemical formula 1 Bmay be at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni, and Zn, x1 in the following chemical formula 1 may be 0.10 or more and 0.90 or less, y1 in the following chemical formula 1 may be 0.05 or more and 0.85 or less, z1 in the following chemical formula 1 may be 0.05 or more and 0.85 or less, x1+y1+z1 may be 1.00, and α in the following chemical formula 1 may be 0.00 or more and less than 1.00. x1(Bi 1-α E A α )E B O3-y1BiFeO3-z1Bi(Fe 0.5 Ti 0.5 )O3(1)

[0014] The tetragonal crystal 2 may be represented by the following chemical formula 2, and E in the following chemical formula 2 A may be at least one element selected from the group consisting of Na, K and Ag, and E in the following chemical formula 2 B may be at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni, and Zn, x2 in the following chemical formula 2 may be 0.10 or more and 0.85 or less, y2 in the following chemical formula 2 may be 0.10 or more and 0.85 or less, z2 in the following chemical formula 2 may be 0.05 or more and 0.80 or less, x2+y2+z2 may be 1.00, and α in the following chemical formula 2 may be 0.00 or more and less than 1.00. x2(Bi 1-α E A α )E B O3-y2BiFeO3-z2Bi(Fe 0.5 Ti 0.5 )O3(2)

[0015] The first piezoelectric layer may have a thickness of not less than 10 nm and not more than 300 nm.

[0016] A piezoelectric thin film element according to one aspect of the present invention includes the above-described piezoelectric thin film.

[0017] A piezoelectric thin film element according to one aspect of the present invention may include a single crystal substrate, an electrode layer overlying the single crystal substrate, and a piezoelectric thin film overlying the electrode layer, and a first intermediate layer may be disposed between the single crystal substrate and the electrode layer, and the first intermediate layer may contain ZrO2 and Y2O3.

[0018] A piezoelectric thin film element according to one aspect of the present invention may include an electrode layer and a piezoelectric thin film overlying the electrode layer, a second intermediate layer may be disposed between the electrode layer and the piezoelectric thin film, and the second intermediate layer may include at least one of SrRuO3 and LaNiO3.

[0019] A piezoelectric thin film element according to one aspect of the present invention may comprise an electrode layer and a piezoelectric thin film overlying the electrode layer, the electrode layer may contain platinum crystals, the (002) plane of the platinum crystals may be oriented in a normal direction to a surface of the electrode layer, and the (200) plane of the platinum crystals may be oriented in an in-plane direction to the surface of the electrode layer.

[0020] A piezoelectric transducer according to one aspect of the present invention includes the above-described piezoelectric thin film element. Effect of the Invention

[0021] According to one aspect of the present invention, there is provided a piezoelectric thin film having a large piezoelectric figure of merit, a piezoelectric thin film element including the piezoelectric thin film, and a piezoelectric transducer. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1(a) is a schematic cross-sectional view of a piezoelectric thin film element according to one embodiment of the present invention, and FIG. 1(b) is an exploded perspective view of the piezoelectric thin film element shown in FIG. 1(a). [Diagram 2] FIG. 2 is a perspective view of a unit cell of a perovskite structure (perovskite oxide), showing the arrangement of each element in the perovskite structure. [Diagram 3] FIG. 3 is a schematic perspective view of the unit cells of the tetragonal crystal 1 and the tetragonal crystal 2. [Figure 4]FIG. 4 is a schematic cross-sectional view of a piezoelectric thin film element (ultrasonic transducer) according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] A preferred embodiment of the present invention will be described in detail below with reference to the drawings. However, the present invention is not limited to the following embodiment. In the drawings, the same or equivalent elements are given the same reference numerals. The X-axis, Y-axis, and Z-axis shown in Fig. 1(a), Fig. 1(b), and Fig. 4 are three coordinate axes that are perpendicular to each other. The directions of the three coordinate axes are common to Fig. 1(a), Fig. 1(b), and Fig. 4.

[0024] The piezoelectric thin film element according to this embodiment includes a piezoelectric thin film. (a) in FIG. 1 shows a cross section of a piezoelectric thin film element 10 according to this embodiment. The cross section of the piezoelectric thin film element 10 is perpendicular to the surface of the piezoelectric thin film 3. The piezoelectric thin film element 10 may have a single crystal substrate 1, a first electrode layer 2 (lower electrode layer) overlapping the single crystal substrate 1, a piezoelectric thin film 3 overlapping the first electrode layer 2, and a second electrode layer 4 (upper electrode layer) overlapping the piezoelectric thin film 3. The piezoelectric thin film element 10 may further include a first intermediate layer 5. The first intermediate layer 5 may be disposed between the single crystal substrate 1 and the first electrode layer 2, and the first electrode layer 2 may directly overlap the surface of the first intermediate layer 5. The piezoelectric thin film element 10 may further include a second intermediate layer 6. The second intermediate layer 6 may be disposed between the first electrode layer 2 and the piezoelectric thin film 3, and the piezoelectric thin film 3 may directly overlap the surface of the second intermediate layer 6. The thickness of each of the single crystal substrate 1, the first intermediate layer 5, the first electrode layer 2, the second intermediate layer 6, the piezoelectric thin film 3, and the second electrode layer 4 may be uniform. As shown in FIG. 1(b), the normal direction dn of the surface of the piezoelectric thin film 3 is perpendicular to the normal direction D N The normal direction dn to the surface of the piezoelectric thin film 3 may be rephrased as the thickness direction of the piezoelectric thin film 3. In (b) of FIG. 1, the first electrode layer, the first intermediate layer, the second intermediate layer, and the second electrode layer are omitted.

[0025] The modified piezoelectric thin film element 10 may not include the single crystal substrate 1. For example, the single crystal substrate 1 may be removed after the first electrode layer 2 and the piezoelectric thin film 3 are formed. The modified piezoelectric thin film element 10 may not include the second electrode layer 4. For example, the piezoelectric thin film element without the second electrode layer may be supplied to an electronic device manufacturer as a product, and then the second electrode layer may be added to the piezoelectric thin film element during the manufacturing process of the electronic device. When the single crystal substrate 1 functions as an electrode, the modified piezoelectric thin film element 10 may not include the first electrode layer 2. That is, the modified piezoelectric thin film element 10 may include the single crystal substrate 1 and the piezoelectric thin film 3 overlapping the single crystal substrate 1. If there is no first electrode layer 2, the piezoelectric thin film 3 may directly overlap the single crystal substrate 1. If there is no first electrode layer 2, the piezoelectric thin film 3 may overlap the single crystal substrate 1 via at least one intermediate layer of the first intermediate layer 5 and the second intermediate layer 6.

[0026] The piezoelectric thin film 3 includes a first piezoelectric layer 3A overlapping the first electrode layer 2 and a second piezoelectric layer 3B directly overlapping the first piezoelectric layer 3A. The piezoelectric thin film 3 may be composed of only the first piezoelectric layer 3A and the second piezoelectric layer 3B. The first piezoelectric layer 3A includes a tetragonal crystal 1 (first tetragonal crystal) of a perovskite oxide. The second piezoelectric layer 3B includes a tetragonal crystal 2 (second tetragonal crystal) of a perovskite oxide. Needless to say, a perovskite oxide is an oxide having a perovskite structure. The perovskite oxide is the main component of each of the first piezoelectric layer 3A and the second piezoelectric layer 3B. The total content of elements constituting the perovskite oxide in the first piezoelectric layer 3A may be 99% by mol or more and 100% by mol or less. The total content of elements constituting the perovskite oxide in the second piezoelectric layer 3B may be 99% by mol or more and 100% by mol or less. The first piezoelectric layer 3A may be made of only tetragonal crystals 1. The first piezoelectric layer 3A may not contain tetragonal crystals 2. The first piezoelectric layer 3A may contain a small amount of tetragonal crystals 2. The second piezoelectric layer 3B may be made of only tetragonal crystals 2. The second piezoelectric layer 3B may not contain tetragonal crystals 1. The first piezoelectric layer 3A may contain a small amount of crystals other than tetragonal crystals in addition to tetragonal crystals 1. The second piezoelectric layer 3B may also contain a small amount of crystals other than tetragonal crystals in addition to tetragonal crystals 2. For example, the small amount of crystals other than tetragonal crystals may be at least one type of perovskite oxide crystals selected from the group consisting of cubic crystals and rhombohedral crystals. The tetragonal crystals 1 may be single crystals or polycrystals. The tetragonal crystals 2 may also be single crystals or polycrystals. The composition of the tetragonal crystals 1 may be different from the composition of the tetragonal crystals 2. The composition of tetragonal 1 may be the same as the composition of tetragonal 2.

[0027] The perovskite oxide may contain bismuth (Bi), iron (Fe) and oxygen (O). 2+ (ferrous iron) and Fe 3+ The perovskite oxide may contain both Fe and Fe(III) as iron. 3+ (iron (III)). The perovskite oxide may contain only Bi, Fe, and O, as well as the element E. A may contain element E Amay be at least one element selected from the group consisting of sodium (Na), potassium (K) and silver (Ag). The perovskite oxide is A The perovskite oxide may contain a plurality of elements as Bi, Fe, and O, as well as the element E. B may contain element E B may be at least one element selected from the group consisting of magnesium (Mg), aluminum (Al), zirconium (Zr), titanium (Ti), nickel (Ni) and zinc (Zn). The perovskite oxide is B The perovskite oxide may contain multiple elements such as Bi, Fe, E A , E B The piezoelectric thin film 3 may contain all of Bi, Fe, E, and O. A , E B and may further contain elements other than O. The piezoelectric thin film 3 does not have to contain Pb. The piezoelectric thin film 3 may contain Pb.

[0028] FIG. 2 shows the unit cell uc of a perovskite oxide. In FIG. 2, a, b, and c are the basic vectors of the perovskite structure. The element located at the A site of the unit cell uc is Bi or E. A The element located at the B site of the unit cell uc may be Fe or E. B A part of the Fe at the B site may be divalent iron (Fe 2+ ), and the balance of the Fe at the B site may be trivalent iron (Fe 3+ The Fe at the B site may be trivalent iron (Fe 3+ ) may be used.

[0029] FIG. 3 shows a unit cell uc1 of a tetragonal crystal 1 and a unit cell uc2 of a tetragonal crystal 2. For convenience of illustration, E in the unit cells uc1 and uc2 B Although and O (oxygen) are omitted, the unit cells uc1 and uc2 each have a perovskite structure similar to that of the unit cell uc in FIG.

[0030] a1, b1, and c1 in FIG. 3 are basic vectors of the tetragonal crystal 1. The vector a1 in FIG. 3 corresponds to the vector a in FIG. 2. The vector b1 in FIG. 3 corresponds to the vector b in FIG. 2. The vector c1 in FIG. 3 corresponds to the vector c in FIG. 2. a1, b1, and c1 are perpendicular to each other. The orientation of the vector a1 (a-axis) is

[0100] . The orientation of the vector b1 (b-axis) is

[0010] . The orientation of the vector c1 (c-axis) is

[0001] . The length a1 of the vector a1 is the spacing of the (100) planes of the tetragonal crystal 1 (i.e., the lattice constant in the

[0100] direction). The length b1 of the vector b1 is the spacing of the (010) planes of the tetragonal crystal 1 (i.e., the lattice constant in the

[0010] direction). The length c1 of the vector c1 is the spacing of the (001) planes of the tetragonal crystal 1 (i.e., the lattice constant in the

[0001] direction). Length a1 is equal to length b1. Length c1 is greater than length a1.

[0031] a2, b2, and c2 in FIG. 3 are the basic vectors of the tetragonal crystal 2. The vector a2 in FIG. 3 corresponds to the vector a in FIG. 2. The vector b2 in FIG. 3 corresponds to the vector b in FIG. 2. The vector c2 in FIG. 3 corresponds to the vector c in FIG. 2. a2, b2, and c2 are perpendicular to each other. The orientation of the vector a2 (a-axis) is

[0100] . The orientation of the vector b2 (b-axis) is

[0010] . The orientation of the vector c2 (c-axis) is

[0001] . The length a2 of the vector a2 is the spacing of the (100) planes of the tetragonal crystal 2 (i.e., the lattice constant in the

[0100] direction). The length b2 of the vector b2 is the spacing of the (010) planes of the tetragonal crystal 2 (i.e., the lattice constant in the

[0010] direction). The length c2 of the vector c2 is the spacing of the (001) planes of the tetragonal crystal 2 (i.e., the lattice constant in the

[0001] direction). Length a2 is equal to length b2. Length c2 is greater than length a2.

[0032] As shown in FIG. 1(b) and FIG. 3, the (001) plane of tetragonal crystal 1 (uc1) is oriented in the normal direction dn of the surface of the piezoelectric thin film 3. The (001) plane of tetragonal crystal 2 (uc2) is also oriented in the normal direction dn of the surface of the piezoelectric thin film 3. For example, the (001) plane of tetragonal crystal 1 and the (001) plane of tetragonal crystal 2 may each be approximately parallel to the surface of the piezoelectric thin film 3, and the

[0001] directions of tetragonal crystal 1 and tetragonal crystal 2 may each be approximately parallel to the normal direction dn of the surface of the piezoelectric thin film 3. The (001) plane of tetragonal crystal 1 is oriented in the normal direction Dn of the surface of the single crystal substrate 1. N The (001) plane of the tetragonal crystal 2 may be oriented in the normal direction D of the surface of the single crystal substrate 1. N In other words, the (001) plane of the tetragonal crystal 1 and the (001) plane of the tetragonal crystal 2 may be approximately parallel to the surface of the single crystal substrate 1, and the

[0001] directions of the tetragonal crystal 1 and the tetragonal crystal 2 may be aligned in the normal direction D of the surface of the single crystal substrate 1. N It may be approximately parallel to.

[0033] The tetragonal crystal of the perovskite oxide is easily polarized in the

[0001] direction. In other words,

[0001] is an orientation in which the tetragonal crystal of the perovskite oxide is easily polarized compared to other crystal orientations. Therefore, the (001) plane of the tetragonal crystal 1 and the (001) plane of the tetragonal crystal 2 are each oriented in the normal direction dn of the surface of the piezoelectric thin film 3, so that the piezoelectric thin film 3 can have excellent piezoelectric properties. For the same reason, the piezoelectric thin film 3 may be a ferroelectric material. The crystal orientation described below means that the (001) plane of the tetragonal crystal 1 and the (001) plane of the tetragonal crystal 2 are each oriented in the normal direction dn of the surface of the piezoelectric thin film 3.

[0034] Since the piezoelectric thin film 3 has the above-mentioned crystal orientation, the piezoelectric thin film 3 has a large (-e 31,f ) 2 / ε0ε r(piezoelectric figure of merit). The above crystal orientation is a characteristic inherent to a thin film. A thin film is a crystalline film formed by a vapor phase growth method or a solution method. On the other hand, it is difficult for a bulk of a piezoelectric body having the same composition as the piezoelectric thin film 3 to have the above crystal orientation. This is because the bulk of a piezoelectric body is a sintered body (ceramic) of powder containing essential elements of a piezoelectric body, and it is difficult to control the structure and orientation of the many crystals that make up the sintered body. The bulk of a piezoelectric body contains Fe, so the resistivity of the bulk of the piezoelectric body is lower than that of the piezoelectric thin film 3. As a result, leakage current is likely to occur in the bulk of the piezoelectric body. Therefore, it is difficult to polarize the bulk of a piezoelectric body by applying a high electric field, and it is difficult for the bulk of a piezoelectric body to have a large piezoelectric figure of merit.

[0035] The c2 / a2 of the tetragonal crystals 2 contained in the second piezoelectric layer 3B is larger than the c1 / a1 of the tetragonal crystals 1 contained in the first piezoelectric layer 3A.

[0036] Since c2 / a2 is larger than c1 / a1, the dielectric constant of tetragonal crystal 2 is lower than that of tetragonal crystal 1. However, since c2 / a2 is larger than c1 / a1, the crystal structure of tetragonal crystal 2 is stronger than that of tetragonal crystal 1, and the atoms in tetragonal crystal 2 are less likely to move than those in tetragonal crystal 1. Therefore, polarization inversion of tetragonal crystal 2 is less likely to occur than that of tetragonal crystal 1, and the piezoelectricity of tetragonal crystal 2 itself is inferior to that of tetragonal crystal 1 itself. In other words, since c1 / a1 is smaller than c2 / a2, the dielectric constant of tetragonal crystal 1 is higher than that of tetragonal crystal 2, but the crystal structure of tetragonal crystal 1 is softer than that of tetragonal crystal 2, and the atoms in tetragonal crystal 1 are more likely to move than those in tetragonal crystal 2. Therefore, polarization inversion of the tetragonal crystal 1 occurs more easily than polarization inversion of the tetragonal crystal 2, and the piezoelectricity of the tetragonal crystal 1 itself is superior to the piezoelectricity of the tetragonal crystal 2 itself. When an electric field is applied to the piezoelectric thin film 3, the polarization inversion of the tetragonal crystal 1 in the first piezoelectric layer 3A tends to occur before the polarization inversion of the tetragonal crystal 2 in the second piezoelectric layer 3B. Due to the polarization inversion of the tetragonal crystal 1 preceding the polarization inversion of the tetragonal crystal 2, the crystal structure of the tetragonal crystal 2 becomes unstable at the interface between the first piezoelectric layer 3A and the second piezoelectric layer 3B. In other words, due to the polarization inversion of the tetragonal crystal 1, the polarization of the tetragonal crystal 2 tends to fluctuate at the interface between the tetragonal crystal 1 and the tetragonal crystal 2. For example, due to the polarization inversion of the tetragonal crystal 1 in the first piezoelectric layer 3A, the charge on the surface of the first piezoelectric layer 3A repels the charge on the surface of the second piezoelectric layer 3B at the interface between the first piezoelectric layer 3A and the second piezoelectric layer 3B, and the polarization of the tetragonal crystal 2 fluctuates. Due to the above-mentioned mechanism, the polarization inversion of the tetragonal crystal 1 induces the polarization inversion of the tetragonal crystal 2. In other words, by introducing the first piezoelectric layer 3A between the first electrode layer 2 and the second piezoelectric layer 3B as a buffer layer that promotes the polarization inversion of the second piezoelectric layer 3B, the polarization inversion is likely to occur in the entire piezoelectric thin film 3. As a result, the piezoelectricity (-e 31,f ) is higher than the piezoelectricity of the tetragonal crystal 2 itself, resulting in a large -e 31,f and low relative dielectric constant (ε r ) and the piezoelectric thin film 3 is large (-e 31,f ) 2 / ε0ε r (piezoelectric figure of merit). However, the above mechanism is merely a hypothesis, and the technical scope of the present invention is not limited to the above mechanism.

[0037] In contrast to the piezoelectric thin film 3, stress-induced distortion of the crystal structure is unlikely to occur in the bulk of the piezoelectric body. Therefore, most perovskite oxides constituting the bulk of the piezoelectric body are cubic crystals, and it is difficult for the bulk of the piezoelectric body to have piezoelectricity resulting from the tetragonal crystal structure of the perovskite oxide.

[0038] c1 / a1 is 1.015 or more and 1.050 or less. Because c1 / a1 is 1.015 or more and 1.050 or less, the polarization inversion of the tetragonal crystal 1 occurs more easily than the polarization inversion of the tetragonal crystal 2, the piezoelectricity of the tetragonal crystal 1 itself is superior to the piezoelectricity of the tetragonal crystal 2 itself, and the -e 31,fand the piezoelectric figure of merit is large. If c1 / a1 is outside the above range, the relative dielectric constant of the tetragonal crystal 1 becomes too high, or the piezoelectricity of the tetragonal crystal 1 itself deteriorates. As a result, the piezoelectric figure of merit of the piezoelectric thin film 3 decreases. c1 may be, for example, 4.010 Å or more and 4.084 Å or less. a1 may be, for example, 3.890 Å or more and 3.950 Å or less.

[0039] c2 / a2 may be 1.051 or more and 1.250 or less, or 1.051 or more and 1.249 or less. When c2 / a2 is 1.051 or more, the relative dielectric constants of the second piezoelectric layer 3B containing the tetragonal crystal 2 and the piezoelectric thin film 3 are likely to decrease, and the piezoelectric performance index of the piezoelectric thin film 3 is likely to increase. When c2 / a2 is 1.250 or less, polarization inversion of the tetragonal crystal 2 is likely to occur, and the piezoelectric performance index of the piezoelectric thin film 3 is likely to increase. c2 may be, for example, 4.155 Å or more and 4.710 Å or less. a2 may be, for example, 3.770 Å or more and 3.950 Å or less.

[0040] The magnitude relationship between c1 and c2 and the magnitude relationship between a1 and a2 may be determined by observing a cross section of the piezoelectric thin film 3 parallel to the thickness direction of the piezoelectric thin film 3 with atomic level resolution using a scanning transmission electron microscope (STEM). In order to specify the specific values ​​of c1 and c2 with high accuracy, the peak P1 of the diffracted X-rays of the (001) plane of the tetragonal crystal 1 and the peak 2 of the diffracted X-rays of the (001) plane of the tetragonal crystal 2 may be measured by out-of-plane measurement (2θ-θ method) on the surface of the piezoelectric thin film 3. One measured X-ray diffraction pattern includes both the peak P1 and the peak 2. When the diffraction angle 2θ1 of the peak P1 of the diffracted X-rays of the (001) plane of the tetragonal crystal 1 is close to the diffraction angle 2θ2 of the peak P2 of the diffracted X-rays of the (001) plane of the tetragonal crystal 2 and the peak P3 where the peaks P1 and P2 overlap is measured, the peak P1 may be approximated by a Gaussian function g1, the peak P2 may be approximated by another Gaussian function g2, and curve fitting between g1+g2 and the peak P3 may be performed. The g1 after the curve fitting may be regarded as P1, and the g2 after the curve fitting may be regarded as P2. In order to specify the specific values ​​of a1 and a2 with high accuracy, a peak P1' of the diffracted X-rays of the (100) plane of the tetragonal crystal 1 and a peak P2' of the diffracted X-rays of the (100) plane of the tetragonal crystal 2 may be measured by in-plane measurement (2θ-θ method) on the surface of the piezoelectric thin film 3. One measured X-ray diffraction pattern includes both peaks P1' and 2'. When the diffraction angle 2θ1' of the peak P1' of the diffracted X-rays of the (100) plane of the tetragonal crystal 1 is close to the diffraction angle 2θ2' of the peak P2' of the diffracted X-rays of the (100) plane of the tetragonal crystal 2 and a peak P3' where the peaks P1' and P2' overlap is measured, the peak P1' may be approximated by a Gaussian function G1, the peak P2' may be approximated by another Gaussian function G2, and curve fitting between G1+G2 and the peak P3' may be performed. G1 after curve fitting may be considered as P1', and G2 after curve fitting may be considered as P2'.

[0041] I2 / (I1+I2) may be 0.90 or more and less than 1.00, or 0.91 or more and 0.99 or less. I1 is the peak intensity (maximum intensity) of the diffracted X-rays from the (001) plane of the tetragonal crystal 1. I2 is the peak intensity (maximum intensity) of the diffracted X-rays from the (001) plane of the tetragonal crystal 2. As I2 / (I1+I2) increases, -e 31,f The relative dielectric constant (ε r ) tends to decrease. When I2 / (I1+I2) of the piezoelectric thin film 3 is within the above range, a large (-e 31,f ) 2 and low relative dielectric constant (ε r ) is easily achieved, and the piezoelectric thin film 3 has a large (-e 31,f ) 2 / ε0ε r (piezoelectric figure of merit). The units of I1 and I2 may be, for example, cps (counts per second). I1 and I2 may be measured by out-of-plane measurement on the surface of the piezoelectric thin film 3. The measurement conditions for I1 and I2 may be set so that I1 and I2 are at least three orders of magnitude higher than the background intensity.

[0042] I1 may be proportional to the total area of ​​the (001) planes of the tetragonal crystals 1 oriented in the normal direction dn of the surface of the piezoelectric thin film 3, and I2 may be proportional to the total area of ​​the (001) planes of the tetragonal crystals 2 oriented in the normal direction dn of the surface of the piezoelectric thin film 3. In other words, I1 may be proportional to the amount of the tetragonal crystals 1 contained in the piezoelectric thin film 3, and I2 may be proportional to the amount of the tetragonal crystals 2 contained in the piezoelectric thin film 3. Therefore, I2 / (I1+I2) may be the abundance ratio of the tetragonal crystals 2 to the total amount of the tetragonal crystals 1 and tetragonal crystals 2. In other words, the abundance ratio of the tetragonal crystals 2 to the total amount of the tetragonal crystals 1 and tetragonal crystals 2 may be 90% or more and less than 100%.

[0043] The degree of orientation of each of the (001) planes of tetragonal crystal 1 and the (001) planes of tetragonal crystal 2 may be quantified by the degree of orientation. The greater the degree of orientation of each of the (001) planes of tetragonal crystal 1 and the (001) planes of tetragonal crystal 2, the greater the piezoelectric performance index of the piezoelectric thin film 3. The degree of orientation of each crystal plane may be calculated based on the peak of diffracted X-rays originating from each crystal plane. The peak of diffracted X-rays originating from each crystal plane may be measured by out-of-plane measurement on the surface of the piezoelectric thin film 3. The orientation of the (001) plane of the tetragonal crystal 1 in the normal direction dn of the surface of the piezoelectric thin film 3 is 100×I1 / ΣI 1(hkl) It can be expressed as ΣI 1(hkl) is the sum of the peak intensities of the diffracted X-rays of each crystal plane of the tetragonal crystal 1 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. 1(hkl) For example, I 1(001) +I 1(110) +I 1(111) It may be. 1(001) is the above I1. That is, I 1(001) is the peak intensity (maximum intensity) of the diffracted X-rays of the (001) plane of the tetragonal crystal 1 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. 1(110) is the peak intensity (maximum intensity) of the diffracted X-rays of the (110) plane of the tetragonal crystal 1 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. 1(111)is the peak intensity (maximum intensity) of diffracted X-rays from the (111) plane of the tetragonal crystal 1 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. The orientation of the (001) plane of tetragonal crystal 2 is 100×I2 / ΣI 2(hkl) It can be expressed as ΣI 2(hkl) is the sum of the peak intensities of the diffracted X-rays of each crystal plane of the tetragonal crystal 2 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. 2(hkl) For example, I 2(001) +I 2(110) +I 2(111) It may be. 2(001) is the above mentioned I2. That is, I 2(001) is the peak intensity (maximum intensity) of the diffracted X-rays of the (001) plane of the tetragonal crystal 2 measured in the out-of-plane direction of the surface of the piezoelectric thin film 3. 2(110) is the peak intensity (maximum intensity) of the diffracted X-rays of the (110) plane of the tetragonal crystal 2 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. 2(111) is the peak intensity (maximum intensity) of the diffracted X-rays of the (111) plane of the tetragonal crystal 2 measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. The degree of orientation of each of the (001) plane of the tetragonal crystal 1 and the (001) plane of the tetragonal crystal 2 may be quantified by the degree of orientation F based on the Lotgering method. Regardless of which of the above methods is used to calculate the degree of orientation, the degree of orientation of each of the (001) plane of the tetragonal crystal 1 and the (001) plane of the tetragonal crystal 2 may be 70% or more and 100% or less, preferably 80% or more and 100% or less, and more preferably 90% or more and 100% or less. In other words, the (001) plane of the tetragonal crystal 1 may be oriented in the normal direction dn of the surface of the piezoelectric thin film 3 in preference to other crystal planes of the tetragonal crystal 1, and the (001) plane of the tetragonal crystal 2 may also be oriented in the normal direction dn of the surface of the piezoelectric thin film 3 in preference to other crystal planes of the tetragonal crystal 2.

[0044] One or both of the tetragonal 1 and tetragonal 2 are Fe 2+ One or both of the tetragonal 1 and tetragonal 2 may contain Fe. 2+When Fe is contained, the piezoelectric thin film 3 tends to have a large piezoelectric figure of merit. 2+ The reason why the piezoelectric thin film 3 is likely to have a large piezoelectric figure of merit is not limited to the following. When the piezoelectric thin film of BiFeO3-(Bi,K)TiO3 system has a composition near the morphotropic phase boundary (MPB) between tetragonal and rhombohedral crystals, the piezoelectricity (-e 31,f ) is improved, but the dielectric constant (ε0ε r ) also increases, so the piezoelectric figure of merit is difficult to improve. In order to suppress the increase in the dielectric constant, it is desirable to improve the piezoelectricity (ferroelectricity) of the piezoelectric thin film by constructing the piezoelectric thin film only from tetragonal crystals. The tetragonality of the piezoelectric thin film is realized by epitaxial stress (compressive stress due to lattice mismatch). This is because the epitaxial stress parallel to the surface of the piezoelectric thin film compresses the piezoelectric thin film in directions parallel to the surface of the piezoelectric thin film (i.e., the a-axis direction and the b-axis direction), distorting the piezoelectric thin film. However, the thicker the piezoelectric thin film is, the more difficult it is to improve the tetragonality of the piezoelectric thin film only by epitaxial stress. This is because the thicker the piezoelectric thin film is, the more difficult it is to distort the entire piezoelectric thin film by epitaxial stress. Therefore, even if the piezoelectric thin film is so thick that the epitaxial stress generated in the piezoelectric thin film is weakened, it is desirable to stabilize the tetragonal structure of the piezoelectric thin film. Therefore, in either or both of tetragonal 1 and tetragonal 2, the electron configuration of the element (ion) located at the B site of the perovskite oxide is the Co that constitutes BiCoO3. 3+ The B site ion is Fe, so that the d6 electron configuration is similar to that of 2+ As a result, even if the piezoelectric thin film 3 is so thick that the epitaxial stress generated in the piezoelectric thin film 3 is weakened, the tetragonality of the piezoelectric thin film 3 is improved. In other words, even if the piezoelectric thin film 3 is so thick that the epitaxial stress generated in the piezoelectric thin film 3 is weakened, the first piezoelectric layer 3A is likely to contain tetragonal crystals 1 and the second piezoelectric layer 3B is likely to contain tetragonal crystals 2. Even in the case of compositions near the MPB where rhombohedral crystals are expected to form in the piezoelectric bulk, some of the B sites are Fe.2+ Although rotation (rotation around the c-axis) of the BO6 octahedron (or BO5 pyramid) in the tetragonal crystal substituted with Fe can occur, polarization rotation due to the formation of a pseudocubic crystal is suppressed. In other words, when part of the B site is Fe 2+ In the perovskite oxide substituted with , the MPB is unlikely to exist, and polarization rotation in which the direction of the c-axis of the tetragonal crystal changes is unlikely to occur. Due to the above mechanism, one or both of tetragonal 1 and tetragonal 2 are Fe 2+ If it contains, piezoelectricity (-e 31,f ) and dielectric constant (ε0ε r ) is likely to be compatible with each other, and the piezoelectric figure of merit is likely to increase. However, Fe 2+ The above mechanism is hypothetical, and the technical scope of the present invention is Fe 2+ However, the present invention is not limited by the above mechanism.

[0045] In contrast to the piezoelectric thin film 3, stress-induced distortion of the crystal structure is unlikely to occur in the bulk of the piezoelectric body. Therefore, most perovskite oxides constituting the bulk of the piezoelectric body are cubic crystals, and it is difficult for the bulk of the piezoelectric body to have piezoelectricity resulting from the tetragonal crystal structure of the perovskite oxide.

[0046] The thickness Tp of the piezoelectric thin film 3 may be equal to the sum of the thickness Ta of the first piezoelectric layer 3A and the thickness Tb of the second piezoelectric layer 3B. The thickness Tb of the second piezoelectric layer 3B may be greater than the thickness Ta of the first piezoelectric layer 3A. The thickness Tp of the piezoelectric thin film 3 may be 500 nm or more and 5000 nm or less. The thickness Ta of the first piezoelectric layer 3A may be 10 nm or more and 300 nm or less, or 80 nm or more and 300 nm or less. The thickness Tb of the second piezoelectric layer 3B may be 490 nm or more and 4700 nm or less, or 420 nm or more and 4700 nm or less. When the thickness Ta of the first piezoelectric layer 3A is 10 nm or more, the polarization inversion of the tetragonal crystal 1 in the first piezoelectric layer 3A is likely to induce the polarization inversion of the tetragonal crystal 2 in the second piezoelectric layer 3B. As a result, the piezoelectric thin film 3 is likely to have a large piezoelectric performance index. When the thickness Ta of the first piezoelectric layer 3A is 300 nm or less, the relative dielectric constant of the piezoelectric thin film 3 is likely to decrease, and the piezoelectric performance index of the piezoelectric thin film 3 is likely to increase. Even when the thickness Tp of the piezoelectric thin film 3 is 500 nm or more and the piezoelectric thin film 3 is thick, the ions located at the B site of the perovskite oxide are Fe 2+ By being replaced with, the piezoelectric thin film 3 is likely to have a large piezoelectric performance index. By adjusting the thickness Tp of the piezoelectric thin film 3 to 5000 nm or less, the tetragonal crystal 1 and the tetragonal crystal 2 are likely to be formed without relying on epitaxial stress, and the piezoelectric thin film 3 is likely to have a large piezoelectric performance index. Ta, Tb, and Tp are not limited to the above ranges. The measurement method of Ta, Tb, and Tp is not limited. For example, the thickness Tp of the piezoelectric thin film 3 may be measured by a scanning electron microscope (SEM) on a cross section of the piezoelectric thin film 3 parallel to the normal direction dn of the piezoelectric thin film 3. Based on the difference in composition or the magnitude relationship between c1 / a1 and c2 / a2, the first piezoelectric layer 3A and the second piezoelectric layer 3B may be identified on the cross section of the piezoelectric thin film 3, and the thickness Ta of the first piezoelectric layer 3A and the thickness Tb of the second piezoelectric layer 3B may be measured by SEM on the cross section of the piezoelectric thin film 3. The thickness Tp of the piezoelectric thin film 3, the thickness Ta of the first piezoelectric layer 3A, and the thickness Tb of the second piezoelectric layer 3B may each be approximately uniform.

[0047] The tetragonal crystal 1 may be represented by the following Chemical Formula 1. The following Chemical Formula 1 is substantially the same as the following Chemical Formula 1a. x1(Bi 1-α E Aα )E B O3-y1BiFeO3-z1Bi(Fe 0.5 Ti 0.5 )O3(1) (Bi x1(1-α)+y1+z1 E A x1α )(E B x1 Fe y1+0.5z1 Ti 0.5z1 )O 3±δ (1a)

[0048] In the above chemical formula 1, x1+y1+z1 may be 1.00. A is the element described above. E in the above chemical formula 1 B is an element as described above.

[0049] In the above formula 1, (Bi 1-α E A α )E B The Bi that composes O3 is trivalent Bi (Bi 3+ ) or pentavalent Bi (Bi 5+ ) in the above chemical formula 1. 1-α E A α )E B E that constitutes O3 A The sum of the valences (ionic valences) of V A (Bi 1-α E A α )E B E that constitutes O3 B The sum of the valences (ionic valences) of V B In chemical formula 1, (Bi 1-α E A α )E B Bi and E that compose O3 A and E B The sum of the valences is 3(1-α)+V A α+V B , or 5(1-α)+V A α+V B It is expressed as 3(1-α)+V A α+V B , or 5(1-α)+VA α+V B may be +6 to balance the sum of the valences (ionic valences) of O (-6). 3(1-α)+V A α or 5(1-α)+V A α may be +3. B The element E in the above formula 1 may be +3. B The two elements corresponding to element E B1 and element E B2 In this case, the above formula 1 is substantially the same as the following formula 1'. In the following formula 1', β may be 0.00 or more and 1.00 or less. E B1 The valence (ionic valence) of is V B1 It is expressed as E B2 The valence (ionic valence) of is V B2 It is expressed as E B The sum of the valences (ionic valences) of V B is (1-β)V B1 +βV B2 It is expressed as (1-β)V B1 +βV B2 may be +3. x1(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y1BiFeO3‐z1Bi(Fe 0.5 Ti 0.5 )O3(1')

[0050] Bi in the above formula 1a x1(1-α)+y1+z1 E A x1α corresponds to the element located at the A site of the perovskite structure. B x1 Fe y1+0.5z1 Ti 0.5z1 corresponds to an element located at the B site of the perovskite structure.

[0051] The valence of Fe constituting y1BiFeO3 in the above chemical formula 1 is 3, but z1Bi(Fe 0.5 Ti 0.5The valence of Fe constituting O3 is 2. Therefore, the Bi, E A , E B The molar ratios of Bi, E, Fe and Ti are the same as those in the above chemical formula 1. A , E B The composition of the raw material for the first piezoelectric layer 3A is adjusted so that the molar ratio of Fe, Ti, and Fe is the same as that of the tetragonal crystal 1. 2+ may include.

[0052] In the above chemical formula 1, x1 may be 0.10 or more and 0.90 or less, or 0.15 or more and 0.85 or less. When x1 is 0.10 or more and 0.90 or less, the tetragonal crystal 1 is likely to have the above crystal orientation, and c1 / a1 is likely to fall within the above range.

[0053] In the above chemical formula 1, y1 may be 0.05 to 0.85, or 0.05 to 0.80. When y1 is 0.05 to 0.85, the tetragonal crystal 1 is likely to have the above crystal orientation, and c1 / a1 is likely to fall within the above range.

[0054] In the above chemical formula 1, z1 may be 0.05 or more and 0.85 or less, or 0.05 or more and 0.80 or less. When z1 is 0.05 or more and 0.85 or less, the tetragonal crystal 1 is likely to have the above crystal orientation, and c1 / a1 is likely to fall within the above range.

[0055] In the above chemical formula 1, α may be 0.00 or more and less than 1.00. Since the tetragonal crystal 1 is likely to have the above crystal orientation and c1 / a1 is likely to fall within the above range, α may be 0.50. As described above, β in the above chemical formula 1' may be 0.00 or more and 1.00 or less, or greater than 0.00 and less than 1.00. Since the tetragonal crystal 1 is likely to have the above crystal orientation and c1 / a1 is likely to fall within the above range, β may be 0.50.

[0056] δ in the above chemical formula 1a may be 0 or more. As long as the crystal structure of the tetragonal crystal 1 (perovskite structure) is maintained, δ may be a value other than 0. For example, δ may be greater than 0 and less than or equal to 1.0. δ may be calculated, for example, from the valence of each ion located at the A site and the B site of the tetragonal crystal 1. The valence of each ion may be measured by X-ray photoelectron spectroscopy (XPS).

[0057] Bi and E contained in tetragonal 1 A The total number of moles of Fe, Ti and E contained in the tetragonal crystal may be expressed as [A]1. B The total number of moles may be expressed as [B]1, and [A]1 / [B]1 may be 1.0. As long as the tetragonal crystal structure (perovskite structure) is maintained, [A]1 / [B]1 may be a value other than 1.0. In other words, [A]1 / [B]1 may be less than 1.0, and [A]1 / [B]1 may be greater than 1.0.

[0058] The tetragonal crystal 2 may be represented by the following Chemical Formula 2. The following Chemical Formula 2 is substantially the same as the following Chemical Formula 2a. x2(Bi 1-α E A α )E B O3-y2BiFeO3-z2Bi(Fe 0.5 Ti 0.5 )O3(2) (Bi x2(1-α)+y2+z2 E A x2α )(E B x2 Fe y2+0.5z2 Ti 0.5z2 )O 3±δ (2a)

[0059] In the above chemical formula 2, x2+y2+z2 may be 1.00. A is the element described above. E in the above chemical formula 2 B is the element described above. E in the above chemical formula 2 A is E in the above chemical formula 1 A E in the above formula 2 may be the same as or different from EB is E in the above chemical formula 1 B The valence of each element in the above chemical formula 2 may be the same as the valence of each element in the above chemical formula 1. The element E in the above chemical formula 2 may be the same as the valence of each element in the above chemical formula 1. B The two elements corresponding to element E B1 and element E B2 In this case, the above Chemical Formula 2 is substantially the same as the following Chemical Formula 2': β in the following Chemical Formula 2' may be 0.00 or more and 1.00 or less. x2(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y2BiFeO3‐z2Bi(Fe 0.5 Ti 0.5 )O3(2')

[0060] Bi in the above formula 2a x2(1-α)+y2+z2 E A x2α corresponds to the element located at the A site of the perovskite structure. B x2 Fe y2+0.5z2 Ti 0.5z2 corresponds to an element located at the B site of the perovskite structure.

[0061] The valence of Fe constituting y2BiFeO3 in the above chemical formula 2 is 3, but the valence of Fe in z2Bi(Fe 0.5 Ti 0.5 The valence of Fe constituting O3 is 2. Therefore, the Bi, E A , E B The molar ratios of Bi, E, Fe and Ti are the same as those in the above chemical formula 2. A , E B The composition of the raw material of the second piezoelectric layer 3B is adjusted so that the molar ratio of Fe, Ti and Fe is the same as that of the tetragonal crystal 2. 2+ may include.

[0062] In the above chemical formula 2, x2 may be 0.10 or more and 0.85 or less, or 0.10 or more and 0.80 or less. When x2 is 0.10 or more and 0.85 or less, the tetragonal crystal 2 is likely to have the above crystal orientation, and c2 / a2 is likely to fall within the above range.

[0063] In the above chemical formula 2, y2 may be 0.10 or more and 0.85 or less. When y2 is 0.10 or more and 0.85 or less, the tetragonal crystal 2 is likely to have the above crystal orientation, and c2 / a2 is likely to fall within the above range.

[0064] In the above chemical formula 2, z2 may be 0.05 or more and 0.80 or less. When z2 is 0.05 or more and 0.80 or less, the tetragonal crystal 2 is likely to have the above crystal orientation, and c2 / a2 is likely to fall within the above range.

[0065] In the above chemical formula 2, α may be 0.00 or more and less than 1.00. Since the tetragonal crystal 2 is likely to have the above crystal orientation and c2 / a2 is likely to fall within the above range, α may be 0.50. As described above, β in the above chemical formula 2' may be 0.00 or more and 1.00 or less, or greater than 0.00 and less than 1.00. Since the tetragonal crystal 2 is likely to have the above crystal orientation and c2 / a2 is likely to fall within the above range, β may be 0.50.

[0066] δ in the above chemical formula 2a may be 0 or more. As long as the crystal structure of the tetragonal crystal 2 (perovskite structure) is maintained, δ may be a value other than 0. For example, δ may be greater than 0 and less than or equal to 1.0. δ may be calculated, for example, from the valence of each ion located at the A site and the B site of the tetragonal crystal 2. The valence of each ion may be measured by the XPS method.

[0067] Bi and E contained in tetragonal 2 A The total number of moles of Fe, Ti and E contained in the tetragonal crystal 2 may be expressed as [A]2. BThe total number of moles of may be expressed as [B]2, and [A]2 / [B]2 may be 1.0. As long as the tetragonal crystal structure (perovskite structure) is maintained, [A]2 / [B]2 may be a value other than 1.0. In other words, [A]2 / [B]2 may be less than 1.0, and [A]2 / [B]2 may be greater than 1.0.

[0068] The tetragonal crystal 1 may be represented by the following chemical formula 1w. A is the element described above. E in the following chemical formula 1w B is the element described above. In the following chemical formula 1w, w1 may be 0.30 or more and 0.80 or less. In the following chemical formula 1w, α may be 0.00 or more and less than 1.00. (1-w1)Bi 1-α E A α E B O3‐w1BiFeO3(1w)

[0069] The tetragonal crystal 2 may be represented by the following chemical formula 2w. A is the element described above. E in the following chemical formula 2w B is the element described above. In the following chemical formula 2w, w2 may be 0.30 or more and 0.80 or less. In the following chemical formula 2w, α may be 0.00 or more and less than 1.00. E in the following chemical formula 2w A is E in the above chemical formula 1w A E in the following chemical formula 2w may be the same as or different from B is E in the above chemical formula 1w B It may be the same as or different from. (1-w2)Bi 1-α E A α E B O3‐w2BiFeO3(2w)

[0070] The piezoelectric thin film 3 may be an epitaxial film. That is, the piezoelectric thin film 3 may be formed by epitaxial growth. By epitaxial growth, a piezoelectric thin film 3 having excellent anisotropy and crystal orientation is easily formed.

[0071] The surface area of ​​the piezoelectric thin film 3 is, for example, 1 μm 2 More than 500mm 2 The area of ​​each of the single crystal substrate 1, the first intermediate layer 5, the first electrode layer 2, the second intermediate layer 6, and the second electrode layer 4 may be the same as the area of ​​the piezoelectric thin film 3.

[0072] The composition of the piezoelectric thin film 3 may be analyzed by, for example, X-ray fluorescence analysis (XRF), inductively coupled plasma (ICP) emission spectroscopy, and photoelectron spectroscopy (XPS). As a method for identifying the composition and thickness of each of the first piezoelectric layer 3A and the second piezoelectric layer 3B, the composition of the piezoelectric thin film 3 may be analyzed along the thickness direction of the piezoelectric thin film 3 by XPS. For example, the composition of the surface of the piezoelectric thin film 3 may be continuously measured by XPS while uniformly reducing the thickness Tp of the piezoelectric thin film 3 by ion milling or sputtering the surface of the piezoelectric thin film 3. The composition of the cross section of the piezoelectric thin film 3 may be analyzed along the thickness direction of the piezoelectric thin film 3. An energy dispersive X-ray analysis (EDS) device provided in a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM) may be used to analyze the composition of the cross section of the piezoelectric thin film 3 along the thickness direction of the piezoelectric thin film 3. The crystal structure and crystal orientation of each of the first piezoelectric layer 3A and the second piezoelectric layer 3B may be identified by X-ray diffraction (XRD). The crystal structure and crystal orientation of each of the first piezoelectric layer 3A and the second piezoelectric layer 3B described above may be the crystal structure and crystal orientation at room temperature.

[0073] The process of forming the piezoelectric thin film 3 includes a first film formation process and a second film formation process following the first film formation process. In the first film formation process, a first piezoelectric layer 3A is formed by a pulsed-laser deposition (PLD) method using a first target. In the second film formation process, a second piezoelectric layer 3B is formed directly on the surface of the first piezoelectric layer 3A by a PLD method using a second target. The first target is a raw material for the first piezoelectric layer 3A. The first target may be composed of all elements common to the first piezoelectric layer 3A (tetragonal crystal 1). The composition of the first target may be adjusted so that the molar ratio of each element constituting the first target matches the molar ratio of each element constituting the first piezoelectric layer 3A (tetragonal crystal 1). For example, the molar ratio of each element constituting the first target may match the molar ratio of each element constituting the above chemical formula 1. The second target is a raw material for the second piezoelectric layer 3B. The second target may be composed of all elements common to the second piezoelectric layer 3B (tetragonal crystal 2). The composition of the second target may be adjusted so that the molar ratio of each element constituting the second target matches the molar ratio of each element constituting the second piezoelectric layer 3B (tetragonal crystal 2). For example, the molar ratio of each element constituting the second target may match the molar ratio of each element constituting the above chemical formula 2.

[0074] In the PLD method, the elements constituting the target are turned into plasma and evaporated by irradiating the target with pulsed laser light (e.g., excimer laser). According to the PLD method, each element constituting the target can be turned into plasma uniformly in an instant. As a result, the molar ratio of each element in each piezoelectric layer is likely to be approximately the same as the molar ratio of each element in each target, and segregation of elements in each piezoelectric layer is likely to be suppressed. Furthermore, according to the PLD method, each piezoelectric layer is likely to grow epitaxially, and each piezoelectric layer that is dense at the atomic level is likely to be formed. In the PLD method, the growth rate of each piezoelectric layer, and the anisotropy and crystal orientation of the tetragonal crystal constituting each piezoelectric layer can be controlled by changing the pulse number (repetition frequency) of the pulsed laser light. As the repetition frequency of the pulsed laser light decreases, the growth rate of each piezoelectric layer decreases, and the anisotropy and crystal orientation of the tetragonal crystal constituting each piezoelectric layer increase.

[0075] The repetition frequency f2 of the pulsed laser light in the second film formation process is smaller than the repetition frequency f1 of the pulsed laser light in the first film formation process. Since f2 is smaller than f1, it is possible to form a piezoelectric thin film 3 in which c2 / c2 of the tetragonal crystal 2 is larger than c1 / c1 of the tetragonal crystal 1. For example, the repetition frequency f1 of the pulsed laser light in the first film formation process may be 20 Hz. By adjusting f1 to 20 Hz, it is easy to control c1 / a1 of the tetragonal crystal 1 in the first piezoelectric layer 3A to 1.015 or more and 1.050 or less. For example, the repetition frequency f2 of the pulsed laser light in the second film formation process may be 10 Hz. By adjusting f2 to 10 Hz, it is easy to control c2 / a2 of the tetragonal crystal 2 in the second piezoelectric layer 3B to a value larger than 1c1 / c1.

[0076] The first and second targets may be prepared separately by the following method.

[0077] As starting materials for each target, e.g., Bi, E A , E B The oxides of Bi, E, and Ti may be used. As the starting materials, instead of oxides, substances that become oxides upon firing, such as carbonates or oxalates, may be used. After these starting materials are sufficiently dried at 100° C. or higher, Bi, E, and Ti are added to the mixture. A , E B Each starting material is weighed out so that the molar ratio of each of the elements E, Fe, and Ti coincides with the molar ratio of each element in each piezoelectric layer. In the first and second film-forming steps, Bi in the target is more likely to volatilize than other elements. Therefore, the molar ratio of Bi in each target may be adjusted to a value higher than the molar ratio of Bi in each piezoelectric layer. A When a raw material containing K is used as the target, K in the target is more likely to volatilize than other elements in the first and second film formation steps, and therefore the molar ratio of K in each target may be adjusted to a value higher than the molar ratio of K in each piezoelectric layer.

[0078] The weighed starting materials are thoroughly mixed in an organic solvent or water. The mixing time may be 5 hours or more and 20 hours or less. The mixing means may be, for example, a ball mill. After the mixed starting materials are thoroughly dried, the starting materials are molded in a press. The molded starting materials are calcinated to obtain a calcine. The calcine temperature may be 750°C or more and 900°C or less. The calcine time may be 1 hour or more and 3 hours or less. The calcine is pulverized in an organic solvent or water. The pulverization time may be 5 hours or more and 30 hours or less. The pulverization means may be a ball mill. After drying the pulverized calcine, the calcine to which a binder solution has been added is granulated to obtain a calcine powder. The calcine powder is press molded to obtain a block-shaped molded body.

[0079] The binder in the block-shaped compact is volatilized by heating the compact. The heating temperature may be 400° C. or more and 800° C. or less. The heating time may be 2 hours or more and 4 hours or less.

[0080] After the binder is evaporated, the molded body is sintered. The sintering temperature may be 800° C. or more and 1100° C. or less. The sintering time may be 2 hours or more and 4 hours or less. The temperature increase rate and the temperature decrease rate of the molded body during the sintering process may be, for example, 50° C. / hour or more and 300° C. / hour or less.

[0081] Through the above steps, the first target and the second target are individually prepared. The average grain size of the crystal grains of the oxide (perovskite oxide) contained in each target may be, for example, 1 μm or more and 20 μm or less. Each target is Fe 3+ However, each target does not necessarily contain Fe 2+ In the first film formation step, Fe derived from the first target may not be included. 3+ By reducing a part of Fe 2+ In the second deposition step, a first piezoelectric layer 3A containing Fe 3+ By reducing a part of Fe 2+A second piezoelectric layer 3B including the above structure can be obtained.

[0082] In the first film formation step, elements constituting the first target are evaporated in a vacuum atmosphere. The evaporated elements are attached and deposited on the surface of either the second intermediate layer 6, the first electrode layer 2, or the single crystal substrate 1, thereby forming the first piezoelectric layer 3A. In the second film formation process following the first film formation process, elements constituting the second target are evaporated in a vacuum atmosphere. The evaporated elements are attached and deposited on the surface of the first piezoelectric layer 3A to form the second piezoelectric layer 3B.

[0083] In the first film formation step, the first piezoelectric layer 3A may be formed while heating the single crystal substrate 1 and the first electrode layer 2 in a vacuum chamber. The temperature (film formation temperature) of the single crystal substrate 1 and the first electrode layer 2 may be, for example, 450° C. or higher and 600° C. or lower. By setting the film formation temperature to 450° C. or higher, the Fe ions derived from the first target can be easily formed. 3+ Part of the Fe is easily reduced. 2+ When the deposition temperature is less than 450° C., the first piezoelectric layer 3A containing Fe derived from the target is easily formed. 3+ is difficult to reduce, and Fe 2+ It is difficult to obtain a first piezoelectric layer 3A containing Bi. The higher the film formation temperature, the more improved the cleanliness of the surface of the single crystal substrate 1 or the first electrode layer 2, the higher the crystallinity of the first piezoelectric layer 3A, and the more likely it is that the degree of orientation of the crystal plane of the tetragonal system 1 will increase. If the film formation temperature is too high, the elements constituting the first piezoelectric layer 3A will be excessively reduced, making it difficult to obtain a first piezoelectric layer 3A having a desired composition. Furthermore, if the film formation temperature is too high, Bi or K will be easily desorbed from the first piezoelectric layer 3A, making it difficult to control the composition of the first piezoelectric layer 3A.

[0084] The oxygen partial pressure in the vacuum chamber may be, for example, 0.1 Pa or more and 3.0 Pa or less, preferably 0.1 Pa or more and 1.0 Pa or less, and more preferably 0.1 Pa or more and 0.5 Pa or less. By maintaining the oxygen partial pressure within the above range, Fe derived from the target can be easily removed. 3+ Part of the Fe is easily reduced. 2+If the oxygen partial pressure is too low, the elements derived from the target are unlikely to be sufficiently oxidized, making it difficult to form a perovskite-type oxide, and the orientation of the crystal planes of the tetragonal crystal 1 is likely to decrease. If the oxygen partial pressure is too high, the Fe 3+ is difficult to reduce, and Fe 2+ If the oxygen partial pressure is too high, the growth rate of first piezoelectric layer 3A is likely to decrease, and the degree of orientation of the crystal plane of tetragonal system 1 is likely to decrease.

[0085] In the first film formation step, parameters such as the number of times the first target is irradiated with the pulsed laser light (film formation time) and the distance between the single crystal substrate 1 and the first target may be controlled in addition to the repetition frequency f1 of the pulsed laser light. As the number of times the first target is irradiated with the pulsed laser light (film formation time) increases, the thickness of the first piezoelectric layer 3A tends to increase. As the distance between the single crystal substrate 1 and the first target decreases, the thickness and growth rate of the first piezoelectric layer 3A tend to increase.

[0086] Except for the composition of the target and the repetition frequency of the pulsed laser light, the second film formation process may be carried out in a manner substantially similar to the first film formation process described above.

[0087] After the piezoelectric thin film 3 is formed by the first film formation process and the second film formation process, the piezoelectric thin film 3 may be annealed (heated). The temperature (annealing temperature) of the piezoelectric thin film 3 in the annealing process may be, for example, 300°C to 1000°C, 600°C to 1000°C, or 850°C to 1000°C. Annealing the piezoelectric thin film 3 tends to further improve the piezoelectricity of the piezoelectric thin film 3. In particular, annealing at 850°C to 1000°C tends to improve the piezoelectricity of the piezoelectric thin film 3. However, annealing is not essential. The annealing process may be performed in a reducing atmosphere such as nitrogen gas (N2). Annealing in a reducing atmosphere reduces the Fe in the piezoelectric thin film 3 due to the annealing process. 2+ Oxidation of (Fe 3+ The formation of Fe in the piezoelectric thin film 3 is suppressed. 2+ is easily maintained.

[0088] In the above-described process of forming the piezoelectric thin film 3 and the subsequent process of lowering the temperature, compressive stress occurs in the piezoelectric thin film 3. The compressive stress compresses the piezoelectric thin film 3 in directions (a-axis direction and b-axis direction) substantially parallel to the surface of the piezoelectric thin film 3. As a result, tetragonal crystals 1 and tetragonal crystals 2 are likely to be formed. The compressive stress is caused, for example, by lattice mismatch between the single crystal substrate 1 and the piezoelectric thin film 3 (first piezoelectric layer 3A), or by a difference in thermal expansion coefficient between the single crystal substrate 1 and the piezoelectric thin film 3 (first piezoelectric layer 3A).

[0089] The single crystal substrate 1 may be, for example, a substrate made of a single crystal of Si, or a substrate made of a single crystal of a compound semiconductor such as GaAs. The single crystal substrate 1 may be a substrate made of a single crystal of an oxide. The single crystal of the oxide may be, for example, MgO or a perovskite-type oxide (for example, SrTiO3). The thickness of the single crystal substrate 1 may be, for example, 10 μm or more and 1000 μm or less. When the single crystal substrate 1 has conductivity, the single crystal substrate 1 functions as an electrode, so that the first electrode layer 2 may not be required. For example, the conductive single crystal substrate 1 may be a single crystal of SrTiO3 doped with niobium (Nb).

[0090] The crystal orientation of the single crystal substrate 1 is the normal direction D of the surface of the single crystal substrate 1. N That is, the surface of the single crystal substrate 1 may be parallel to the crystal plane of the single crystal substrate 1. The single crystal substrate 1 may be a uniaxially oriented substrate. For example, the (100) plane of the single crystal substrate 1 such as Si may be parallel to the surface of the single crystal substrate 1. That is, the

[0100] direction of the single crystal substrate 1 such as Si may be equal to the normal direction D of the surface of the single crystal substrate 1. N may be parallel to

[0091] When the (100) plane of the single crystal substrate 1 such as Si is parallel to the surface of the single crystal substrate 1 , the (001) planes of the tetragonal crystals 1 and 2 tend to be oriented in the normal direction dn to the surface of the piezoelectric thin film 3 .

[0092] As described above, the first intermediate layer 5 may be disposed between the single crystal substrate 1 and the first electrode layer 2. The first intermediate layer 5 may contain, for example, at least one selected from the group consisting of titanium (Ti), chromium (Cr), titanium oxide (TiO2), silicon oxide (SiO2), and zirconium oxide (ZrO2). The first intermediate layer 5 facilitates adhesion of the first electrode layer 2 to the single crystal substrate 1. The first intermediate layer 5 may be crystalline. The crystal plane of the first intermediate layer 5 may be aligned in the normal direction D of the surface of the single crystal substrate 1. N Both the crystal plane of the single crystal substrate 1 and the crystal plane of the first intermediate layer 5 may be oriented in the normal direction D N The method for forming the first intermediate layer 5 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.

[0093] The first intermediate layer 5 may contain ZrO2 and an oxide of a rare earth element. When the first intermediate layer 5 contains ZrO2 and an oxide of a rare earth element, the first electrode layer 2 made of platinum crystals is easily formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is easily oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals is easily oriented in the in-plane direction of the surface of the first electrode layer 2. The rare earth element may be at least one selected from the group consisting of scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).

[0094] The first intermediate layer 5 may contain ZrO2 and Y2O3. For example, the first intermediate layer 5 may be made of yttria-stabilized zirconia (ZrO2 with added Y2O3). The first intermediate layer 5 may have a first layer made of ZrO2 and a second layer made of Y2O3. The first layer made of ZrO2 may be directly laminated on the surface of the single crystal substrate 1. The second layer made of Y2O3 may be directly laminated on the surface of the first layer. The first electrode layer 2 may be directly laminated on the surface of the second layer made of Y2O3. When the first intermediate layer 5 contains ZrO2 and Y2O3, the first piezoelectric layer 3A and the second piezoelectric layer 3B tend to grow epitaxially, and the (001) planes of the tetragonal crystal 1 and the tetragonal crystal 2 tend to be preferentially oriented in the normal direction dn of the surface of the piezoelectric thin film 3. Furthermore, when the first intermediate layer 5 contains ZrO2 and Y2O3, a first electrode layer 2 made of platinum crystals is likely to be formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is likely to be oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals is likely to be oriented in the in-plane direction of the surface of the first electrode layer 2.

[0095] The first electrode layer 2 may be made of at least one metal selected from the group consisting of platinum (Pt), palladium (Pd), rhodium (Rh), gold (Au), ruthenium (Ru), iridium (Ir), molybdenum (Mo), titanium (Ti), tantalum (Ta), and nickel (Ni). The first electrode layer 2 may be made of a conductive metal oxide such as strontium ruthenate (SrRuO3), lanthanum nickelate (LaNiO3), or lanthanum strontium cobaltate ((La,Sr)CoO3). The first electrode layer 2 may be crystalline. The crystal plane of the first electrode layer 2 is aligned in the normal direction D of the single crystal substrate 1. N The crystal plane of the first electrode layer 2 may be substantially parallel to the surface of the single crystal substrate 1. Both the crystal plane of the single crystal substrate 1 and the crystal plane of the first electrode layer 2 may be oriented in the normal direction D N The single crystal substrate 1 may be oriented in the normal direction D NThe crystal plane of the first electrode layer 2 oriented in the plane may be approximately parallel to the (001) plane of each of the tetragonal crystal 1 and the tetragonal crystal 2. The thickness of the first electrode layer 2 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the first electrode layer 2 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the first electrode layer 2 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the first electrode layer 2.

[0096] The first electrode layer 2 may include platinum crystals. The first electrode layer 2 may consist only of platinum crystals. The platinum crystals are cubic crystals having a face-centered cubic lattice structure (fcc structure). The (002) plane of the platinum crystals may be oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals may be oriented in the in-plane direction of the surface of the first electrode layer 2. In other words, the (002) plane of the platinum crystals may be approximately parallel to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals may be approximately perpendicular to the surface of the first electrode layer 2. When the (002) and (200) planes of the platinum crystal constituting the first electrode layer 2 have the above-mentioned orientation, the first piezoelectric layer 3A and the second piezoelectric layer 3B tend to grow epitaxially on the surface of the first electrode layer 2, and the (001) planes of the tetragonal crystal 1 and the tetragonal crystal 2 tend to be preferentially oriented in the normal direction dn to the surface of the piezoelectric thin film 3. The surface of the first electrode layer 2 may be approximately parallel to the surface of the piezoelectric thin film 3. In other words, the normal direction to the surface of the first electrode layer 2 may be approximately parallel to the normal direction dn to the surface of the piezoelectric thin film 3.

[0097] As described above, the second intermediate layer 6 may be disposed between the first electrode layer 2 and the piezoelectric thin film 3. The second intermediate layer 6 may contain, for example, at least one selected from the group consisting of SrRuO3, LaNiO3, and (La,Sr)CoO3. (La,Sr)CoO3 may be, for example, La 0.5 Sr 0.5CoO3. The second intermediate layer 6 may be crystalline. For example, the second intermediate layer 6 may be a laminate composed of at least two buffer layers selected from the group consisting of a layer containing SrRuO3 crystals, a layer containing LaNiO3 crystals, and a layer containing (La,Sr)CoO3 crystals. SrRuO3, LaNiO3, and (La,Sr)CoO3 all have a perovskite structure. Therefore, when the second intermediate layer 6 contains at least one selected from the group consisting of SrRuO3, LaNiO3, and (La,Sr)CoO3, the first piezoelectric layer 3A and the second piezoelectric layer 3B tend to grow epitaxially, and the (001) planes of the tetragonal crystal 1 and the tetragonal crystal 2 tend to be preferentially oriented in the normal direction dn of the surface of the piezoelectric thin film 3. In addition, the piezoelectric thin film 3 (first piezoelectric layer 3A) tends to adhere to the first electrode layer 2 by passing through the second intermediate layer 6. The crystal plane of the second intermediate layer 6 is aligned in the normal direction D of the surface of the single crystal substrate 1. N Both the crystal plane of the single crystal substrate 1 and the crystal plane of the second intermediate layer 6 may be oriented in the normal direction D N The second intermediate layer 6 may be formed by a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.

[0098] The second electrode layer 4 may be made of at least one metal selected from the group consisting of Pt, Pd, Rh, Au, Ru, Ir, Mo, Ti, Ta, and Ni. The second electrode layer 4 may be made of at least one conductive metal oxide selected from the group consisting of LaNiO3, SrRuO3, and (La,Sr)CoO3. The second electrode layer 4 may be crystalline. The crystal plane of the second electrode layer 4 is aligned in the normal direction D of the single crystal substrate 1. N The crystal plane of the second electrode layer 4 may be approximately parallel to the surface of the single crystal substrate 1. NThe crystal plane of the second electrode layer 4 oriented in the plane may be approximately parallel to the (001) plane of each of the tetragonal 1 and tetragonal 2. The thickness of the second electrode layer 4 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the second electrode layer 4 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the second electrode layer 4 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the second electrode layer 4.

[0099] A third intermediate layer may be disposed between the piezoelectric thin film 3 and the second electrode layer 4. The third intermediate layer facilitates adhesion of the second electrode layer 4 to the piezoelectric thin film 3 (second piezoelectric layer 3B). The composition, crystal structure, and formation method of the third intermediate layer may be the same as those of the second intermediate layer.

[0100] At least a part or the entire surface of the piezoelectric thin film element 10 may be covered with a protective film. Covering with a protective film improves the durability (moisture resistance, etc.) of the piezoelectric thin film element 10.

[0101] The piezoelectric thin film element according to this embodiment has a variety of applications. For example, the piezoelectric thin film element may be used in a piezoelectric transducer. That is, the piezoelectric transducer according to this embodiment may include the above-described piezoelectric thin film element. The piezoelectric transducer may be, for example, an ultrasonic transducer such as an ultrasonic sensor. The piezoelectric thin film element may be, for example, a harvester (vibration power generation element). The piezoelectric thin film element according to this embodiment has a large (-e 31,f ) 2 / ε0ε rSince the piezoelectric thin film includes a piezoelectric thin film having a piezoelectric film having a piezoelectric constant, the piezoelectric thin film element is suitable for an ultrasonic transducer or a harvester. The piezoelectric thin film element may be a piezoelectric actuator. The piezoelectric actuator may be used in a head assembly, a head stack assembly, or a hard disk drive. The piezoelectric actuator may be used in a printer head or an inkjet printer device. The piezoelectric actuator may be a piezoelectric switch. The piezoelectric actuator may be used in haptics. That is, the piezoelectric actuator may be used in various devices that require feedback by skin sensation (touch). The device that requires feedback by skin sensation may be, for example, a wearable device, a touch pad, a display, or a game controller. The piezoelectric thin film element may be a piezoelectric sensor. For example, the piezoelectric sensor may be a piezoelectric microphone, a gyro sensor, a pressure sensor, a pulse wave sensor, or a shock sensor. The piezoelectric thin film element may be a filter (SAW filter or BAW filter), an oscillator, or an acoustic multilayer film. The piezoelectric thin film element may be a part or the whole of a micro electro mechanical system (MEMS). For example, the piezoelectric thin film element may be a piezoelectric micromachined ultrasonic transducer (PMUT). For example, a product to which the piezoelectric micromachined ultrasonic transducer is applied may be a biometric sensor or a medical / healthcare sensor (such as a fingerprint sensor or an ultrasonic blood vessel authentication sensor), or a ToF (Time of Flight) sensor.

[0102] FIG. 4 shows a schematic cross section of an ultrasonic transducer 10a including the above-mentioned piezoelectric thin film 3. The cross section of the ultrasonic transducer 10a is perpendicular to the surface of the piezoelectric thin film 3. The ultrasonic transducer 10a may include substrates 1a and 1b, a first electrode layer 2 disposed on the substrates 1a and 1b, a piezoelectric thin film 3 overlapping the first electrode layer 2, and a second electrode layer 4 overlapping the piezoelectric thin film 3. The piezoelectric thin film 3 includes a first piezoelectric layer 3A overlapping the first electrode layer 2 and a second piezoelectric layer 3B overlapping the first piezoelectric layer 3A. An acoustic cavity 1c may be provided below the piezoelectric thin film 3. An ultrasonic signal is transmitted or received by the deflection or vibration of the piezoelectric thin film 3. A first intermediate layer may be interposed between the substrates 1a and 1b and the first electrode layer 2. A second intermediate layer may be interposed between the first electrode layer 2 and the piezoelectric thin film 3.

[0103] The present invention is not limited to the above embodiment. For example, the piezoelectric thin film 3 may include a second piezoelectric layer 3B overlapping the first electrode layer 2 and a first piezoelectric layer 3A directly overlapping the second piezoelectric layer 3B. EXAMPLES

[0104] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.

[0105] Example 1 A single crystal substrate made of Si was used to fabricate the piezoelectric thin film element of Example 1. The (100) plane of Si was parallel to the surface of the single crystal substrate. The single crystal substrate was a square of 20 mm x 20 mm. The thickness of the single crystal substrate was 500 μm.

[0106] In a vacuum chamber, a crystalline first intermediate layer made of ZrO2 and Y2O3 was formed on the entire surface of the single crystal substrate. The first intermediate layer was formed by a sputtering method. The thickness of the first intermediate layer was 30 nm.

[0107] In the vacuum chamber, a first electrode layer made of Pt crystals was formed on the entire surface of the first intermediate layer. The first electrode layer was formed by a sputtering method. The thickness of the first electrode layer was 200 nm. The temperature of the single crystal substrate during the formation of the first electrode layer was maintained at 500°C.

[0108] The XRD pattern of the first electrode layer was measured by out-of-plane measurement on the surface of the first electrode layer. The XRD pattern of the first electrode layer was measured by in-plane measurement on the surface of the first electrode layer. An X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used to measure these XRD patterns. The measurement conditions were set so that the peak intensity in each XRD pattern was at least three orders of magnitude higher than the background intensity. The out-of-plane measurement detected a diffracted X-ray peak of the (002) plane of the Pt crystal. In other words, the (002) plane of the Pt crystal was oriented in the normal direction of the surface of the first electrode layer. The in-plane measurement detected a diffracted X-ray peak of the (200) plane of the Pt crystal. In other words, the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.

[0109] The first piezoelectric layer was formed on the entire surface of the first electrode layer by carrying out the first film-forming process (PLD method) in a vacuum chamber. The repetition frequency f1 of the pulsed laser light in the first film-forming process was adjusted to 20 Hz. The thickness Ta of the first piezoelectric layer was adjusted to the value shown in Table 2 below.

[0110] The composition of the first target used in the first film formation step is represented by the following chemical formula 1A. When the composition of the first target is represented by the following chemical formula 1′, E in the following chemical formula 1′ A is K, and E in the following chemical formula 1' B1 is Ti, and E in the following chemical formula 1' B2 In Example 1, α in the following chemical formula 1' was 0.5, and β in the following chemical formula 1' was zero. In Example 1, x1, y1, and z1 in the following chemical formula 1A had the values ​​shown in Table 1 below. x1(Bi 0.5 K0.5 )TiO3‐y1BiFeO3‐z1Bi(Fe 0.5 Ti 0.5 )O3(1A) x1(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y1BiFeO3‐z1Bi(Fe 0.5 Ti 0.5 )O3(1')

[0111] After the first film formation process, the second film formation process (PLD method) was carried out in a vacuum chamber to form a second piezoelectric layer on the entire surface of the first piezoelectric layer. The repetition frequency f2 of the pulsed laser light in the second film formation process was adjusted to 10 Hz. The thickness Tb of the second piezoelectric layer was adjusted to the value shown in Table 2 below.

[0112] The composition of the second target used in the second film formation step is represented by the following chemical formula 2A. When the composition of the second target is represented by the following chemical formula 2', E in the following chemical formula 2' A is K, and E in the following chemical formula 2' B1 is Ti, and E in the following chemical formula 2' B2 In Example 1, α in the following chemical formula 2' was 0.5, and β in the following chemical formula 2' was zero. In Example 1, x2, y2, and z2 in the following chemical formula 2A had the values ​​shown in Table 1 below. x2(Bi 0.5 K 0.5 )TiO3-y2BiFeO3-z2Bi(Fe 0.5 Ti 0.5 )O3(2A) x2(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y2BiFeO3‐z2Bi(Fe 0.5 Ti 0.5 )O3(2')

[0113] A piezoelectric thin film consisting of a first piezoelectric layer and a second piezoelectric layer was formed by the above-mentioned first and second film formation steps. The thickness Tp of the piezoelectric thin film was the value shown in Table 2 below. The temperature of the single crystal substrate (film formation temperature) in the first and second film formation steps was maintained at 500°C. The oxygen partial pressure in the vacuum chamber in the first and second film formation steps was maintained at 1 Pa.

[0114] While the thickness Tp of the piezoelectric thin film 3 was uniformly reduced by sputtering the surface of the piezoelectric thin film 3, the composition of the surface of the piezoelectric thin film 3 was continuously analyzed by XPS along the thickness direction of the piezoelectric thin film 3. The analysis results showed that the composition of the first piezoelectric layer was consistent with the composition of the first target, and the composition of the second piezoelectric layer was consistent with the composition of the second target.

[0115] The XRD pattern of the piezoelectric thin film was measured by out-of-plane measurement of the surface of the piezoelectric thin film using the above-mentioned X-ray diffractometer. Furthermore, another XRD pattern of the piezoelectric thin film was measured by in-plane measurement of the surface of the piezoelectric thin film. The measurement conditions were set so that each peak intensity in each XRD pattern was at least three orders of magnitude higher than the background intensity. The measurement device and measurement conditions for each XRD pattern were the same as those described above. The cross section of the piezoelectric thin film parallel to the thickness direction of the piezoelectric thin film was observed at atomic level resolution using a scanning transmission electron microscope (STEM).

[0116] The results of the above analysis using an X-ray diffractometer and STEM showed that the piezoelectric thin film had the following characteristics.

[0117] The first piezoelectric layer was made of tetragonal crystals 1 of a perovskite-type oxide. The (001) plane of the tetragonal crystal 1 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. In other words, the degree of orientation of the (001) plane of the tetragonal crystal 1 in the normal direction to the surface of the piezoelectric thin film was 90% or more. As mentioned above, the degree of orientation of the (001) plane of the tetragonal crystal 1 was 100×I 1(001) / (I 1(001) +I 1(110) +I 1(111)) The c1 / a1 of the tetragonal crystal 1 was the value shown in Table 2 below. The second piezoelectric layer was made of tetragonal crystals 2 of a perovskite-type oxide. The (001) plane of the tetragonal crystal 2 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. In other words, the degree of orientation of the (001) plane of the tetragonal crystal 2 in the normal direction to the surface of the piezoelectric thin film was 90% or more. As mentioned above, the degree of orientation of the (001) plane of the tetragonal crystal 2 was 100×I 2(001) / (I 2(001) +I 2(110) +I 2(111) ) The c2 / a2 ratio of the tetragonal crystal 2 was the value shown in Table 2 below. I2 / (I1+I2) had the value shown in Table 2 below. The definition of I2 / (I1+I2) is as described above.

[0118] By the above-mentioned method, a laminate was produced that was composed of a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, and a piezoelectric thin film overlapping the first electrode layer. The following steps were further carried out using this laminate.

[0119] In a vacuum chamber, a second electrode layer made of Pt was formed on the entire surface of the piezoelectric thin film. The second electrode layer was formed by a sputtering method. The temperature of the single crystal substrate during the process of forming the second electrode layer was maintained at 500°C. The thickness of the second electrode layer was 200 nm.

[0120] Through the above steps, a laminate was produced that was composed of a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a piezoelectric thin film overlapping the first electrode layer, and a second electrode layer overlapping the piezoelectric thin film. The laminate structure on the single crystal substrate was then patterned by photolithography. After patterning, the laminate was cut by dicing.

[0121] Through the above steps, a rectangular piezoelectric thin film element of Example 1 was obtained. The piezoelectric thin film element was composed of a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a piezoelectric thin film overlapping the first electrode layer, and a second electrode layer overlapping the piezoelectric thin film. The area of ​​the movable part of the piezoelectric thin film was 20 mm x 1.0 mm.

[0122] <Evaluation of piezoelectricity> The piezoelectric properties of the piezoelectric thin film were evaluated by the following method.

[0123] [Measurement of residual polarization] The polarization hysteresis of the piezoelectric thin film was measured. For the measurement, a device combining an atomic microscope (AFM) and a ferroelectric evaluation system was used. The atomic microscope was an SPA-400 manufactured by Seiko Instruments Inc. The ferroelectric evaluation system was an FCE manufactured by Toyo Corporation. The frequency of the AC voltage used in measuring the hysteresis was 5 Hz. The maximum voltage applied to the piezoelectric thin film during the measurement was 20 V. The remnant polarization Pr of the piezoelectric thin film is shown in Table 2 below. The unit of remnant polarization Pr is μC / cm. 2 It is.

[0124] [Calculation of relative dielectric constant] The capacitance C of the piezoelectric thin film element was measured. The details of the measurement of the capacitance C were as follows. Measurement equipment: Impedance Gain-Phase Analyzer 4194A manufactured by Hewlett Packard Co. Frequency: 10kHz Electric field: 0.1V / μm

[0125] Based on the following formula A, the relative dielectric constant ε r was calculated. r is shown in Table 2 below. C = ε0 × ε r ×(S / d) (A) ε0 in formula A is the dielectric constant of a vacuum (8.854×10 -12 Fm -1) In formula A, S is the surface area of ​​the piezoelectric thin film. In other words, S is the area of ​​the first electrode layer that overlaps the piezoelectric thin film. In formula A, d is the thickness of the piezoelectric thin film.

[0126] [Piezoelectric constant - e 31,f Measurement of Piezoelectric constant of piezoelectric thin film -e 31,f In order to measure, a rectangular sample (cantilever) was prepared as the piezoelectric thin film element. The dimensions of the sample were 3 mm wide x 15 mm long. Except for the dimensions, the sample was the same as the piezoelectric thin film element in Example 1 above. A homemade evaluation system was used for the measurement. One end of the sample was fixed, and the other end of the sample was a free end. While applying a voltage to the piezoelectric thin film in the sample, the displacement of the free end of the sample was measured with a laser. Then, the piezoelectric constant -e was calculated from the following formula B. 31,f was calculated. Note that E in formula B s is the Young's modulus of the single crystal substrate. h s is the thickness of the single crystal substrate. L is the length of the sample (cantilever). ν s is the Poisson's ratio of the single crystal substrate. δ out is the output displacement based on the measured displacement. V in is the voltage applied to the piezoelectric thin film. Piezoelectric constant -e 31,f The frequency of the AC electric field (AC voltage) in the measurement was 100 Hz. The maximum voltage applied to the piezoelectric thin film was 50 V. 31,f The unit is C / m 2 Example 1-e 31,f is shown in Table 2 below. 31,f ) 2 / ε0ε r (Piezoelectric figure of merit) is shown in Table 2 below.

number

[0127] (Examples 2 to 6 and Comparative Examples 1 to 3) The composition of the first target in each of Examples 2 to 6 and Comparative Examples 1 to 3 was different from that of the first target in Example 1. The composition of the first target in each of Examples 2 to 6 and Comparative Examples 1 to 3 is represented by the following chemical formula 1'. E in chemical formula 1' in each of Examples 2 to 6 and Comparative Examples 1 to 3 A , E B1 and E B2 are shown in the following Table 1. α, β, x1, y1 and z1 in Chemical Formula 1′ of each of Examples 2 to 6 and Comparative Examples 1 to 3 are shown in the following Table 1. x1(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y1BiFeO3‐z1Bi(Fe 0.5 Ti 0.5 )O3(1')

[0128] The composition of the second target in each of Examples 2 to 6 and Comparative Examples 1 to 3 was different from that of the second target in Example 1. The composition of the second target in each of Examples 2 to 6 and Comparative Examples 1 to 3 is represented by the following chemical formula 2'. E in chemical formula 2' in each of Examples 2 to 6 and Comparative Examples 1 to 3 A , E B1 and E B2 are shown in Table 1 below. α, β, x2, y2 and z2 in the chemical formula 2′ in each of Examples 2 to 6 and Comparative Examples 1 to 3 are shown in Table 1 below. In each of Examples 2 to 6 and Comparative Examples 1 to 3, E A , E B1 , E B2 , α and β are common to the above chemical formula 1 (first target) and the following chemical formula 2′ (second target). x2(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐y2BiFeO3‐z2Bi(Fe 0.5 Ti 0.5 )O3(2')

[0129] In the case of Comparative Example 1, the repetition frequency f1 of the pulsed laser light in the first film formation step was adjusted to 10 Hz. The composition of the second target in Comparative Example 1 was the same as the composition of the first target in Comparative Example 1, and the composition of the piezoelectric thin film in Comparative Example 1 was uniform.

[0130] The thickness Ta of the first piezoelectric layer in each of Examples 2 to 6 and Comparative Examples 2 and 3 was adjusted to the value shown in the following Table 2. The thickness Tb of the second piezoelectric layer in each of Examples 2 to 6 and Comparative Examples 2 and 3 was adjusted to the value shown in the following Table 2. The thickness Tp of the piezoelectric thin film in each of Examples 2 to 6 and Comparative Examples 1 to 3 was the value shown in the following Table 2.

[0131] Except for the above, the piezoelectric thin film elements of Examples 2 to 6 and Comparative Examples 1 to 3 were fabricated in the same manner as in Example 1.

[0132] The XRD patterns of the first electrode layers of Examples 2 to 6 and Comparative Examples 1 to 3 were measured by the same method as in Example 1. In all of Examples 2 to 6 and Comparative Examples 1 to 3, the (002) plane of the Pt crystals constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystals was oriented in the in-plane direction of the surface of the first electrode layer.

[0133] The compositions of the piezoelectric thin films of Examples 2 to 6 and Comparative Examples 1 to 3 were analyzed by the same method as in Example 1. In each of Examples 2 to 6 and Comparative Examples 2 and 3, the composition of the first piezoelectric layer was consistent with the composition of the first target, and the composition of the second piezoelectric layer was consistent with the composition of the second target. In the case of Comparative Example 1, the uniform composition of the piezoelectric thin film was consistent with the compositions of the first target and the second target.

[0134] The piezoelectric thin films of Examples 2 to 6 and Comparative Examples 1 to 3 were analyzed using an X-ray diffractometer and STEM in the same manner as in Example 1. The piezoelectric thin films of Examples 2 to 6 and Comparative Examples 1 to 3 had the following characteristics. In all of Examples 2 to 6 and Comparative Example 2, the first piezoelectric layer was made of tetragonal crystals 1 of a perovskite-type oxide. In all of Examples 2 to 6 and Comparative Example 2, the second piezoelectric layer was made of tetragonal crystals 2 of a perovskite-type oxide. In the case of Comparative Example 1, tetragonal crystals 1 of a perovskite type oxide and tetragonal crystals 2 of a perovskite type oxide coexisted in a piezoelectric thin film having a uniform composition. In all of Examples 2 to 6 and Comparative Examples 1 and 2, the (001) plane of the tetragonal crystal 1 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. In all of Examples 2 to 6 and Comparative Examples 1 and 2, the (001) plane of the tetragonal crystal 2 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. The c1 / a1 of the tetragonal crystal 1 in each of Examples 2 to 6 and Comparative Examples 1 and 2 was the value shown in Table 2 below. The c2 / a2 ratio of the tetragonal crystal 2 in each of Examples 2 to 6 and Comparative Examples 1 and 2 was the value shown in Table 2 below. The I2 / (I1+I2) values ​​for each of Examples 2 to 6 and Comparative Examples 1 and 2 were as shown in Table 2 below.

[0135] In the analysis of the piezoelectric thin film of Comparative Example 3, two types of tetragonal crystals differing in anisotropy (c / a) were not detected, and only one type of tetragonal crystal made of perovskite oxide was identified. That is, in the case of Comparative Example 3, it was difficult to distinguish the diffracted X-rays originating from the crystal structure of the first piezoelectric layer from the diffracted X-rays originating from the crystal structure of the second piezoelectric layer, and it was difficult to identify the difference in the crystal structure between the first piezoelectric layer and the second piezoelectric layer. The (001) plane of the tetragonal crystal of Comparative Example 3 was preferentially oriented in the normal direction of the surface of the piezoelectric thin film. Only one value (1.037) was identified as the c / a of the tetragonal crystal of Comparative Example 3. The analysis result of Comparative Example 3 suggested that c1 / a1 of the tetragonal crystal 1 constituting the first piezoelectric layer was equal to c2 / a2 of the tetragonal crystal 2 constituting the second piezoelectric layer.

[0136] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin films of Examples 2 to 6 and Comparative Examples 1 to 3 were evaluated. The Pr of each of Examples 2 to 6 and Comparative Examples 1 to 3 is shown in Table 2 below. ε of Examples 2 to 6 and Comparative Examples 1 to 3 ris shown in Table 2 below. -e for each of Examples 2 to 6 and Comparative Examples 1 to 3 31,f is shown in Table 2 below. (-e 31,f ) 2 / ε0ε r is shown in Table 2 below.

[0137] [Table 1]

[0138] [Table 2]

[0139] Comparative Example 4 As shown in Table 3 below, the composition of the first target of Comparative Example 4 was the same as the composition of the first target of Example 1, and the composition of the second target of Comparative Example 4 was the same as the composition of the second target of Example 1.

[0140] In Comparative Example 4, the oxygen partial pressure in the vacuum chamber was maintained at 0.01 Pa in the first and second film-forming steps.

[0141] The thickness Ta of the first piezoelectric layer of Comparative Example 4 was adjusted to the value shown in the following Table 4. The thickness Tb of the second piezoelectric layer of Comparative Example 4 was adjusted to the value shown in the following Table 4. The thickness Tp of the piezoelectric thin film of Comparative Example 4 was the value shown in the following Table 4.

[0142] A piezoelectric thin film element of Comparative Example 4 was produced in the same manner as in Example 1, except for the above points.

[0143] The XRD pattern of the first electrode layer of Comparative Example 4 was measured by the same method as in Example 1. In the case of Comparative Example 4, the (002) plane of the Pt crystal constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.

[0144] The composition of the piezoelectric thin film of Comparative Example 4 was analyzed by the same method as in Example 1. In the case of Comparative Example 4, the composition of the piezoelectric thin film did not match the compositions of the first target and the second target in terms of the oxygen content.

[0145] The piezoelectric thin film of Comparative Example 4 was analyzed using an X-ray diffractometer and STEM in the same manner as in Example 1. Since the piezoelectric thin film of Comparative Example 4 did not have crystallinity or crystal orientation, it was not possible to identify c1 / a1, c2 / a2, and I2 / (I1+I2) in Comparative Example 3.

[0146] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin film of Comparative Example 4 were evaluated. Pr of Comparative Example 4 is shown in Table 4 below. ε of Comparative Example 4 r is shown in Table 4 below. Comparative Example 4-e 31,f is shown in Table 4 below. Comparative Example 4 (-e 31,f ) 2 / ε0ε r is shown in Table 4 below.

[0147] [Table 3]

[0148] [Table 4]

[0149] (Examples 7 and 8) As shown in Table 5 below, the composition of the first target in each of Examples 7 and 8 was the same as the composition of the first target in Example 1, and the composition of the second target in each of Examples 7 and 8 was the same as the composition of the second target in Example 1.

[0150] In the case of Examples 7 and 8, the second intermediate layer was formed on the entire surface of the first electrode layer, and the first piezoelectric layer was formed on the entire surface of the second intermediate layer. The second intermediate layer of Example 7 was made of crystalline SrRuO3. The thickness of the second intermediate layer of Example 7 was 50 nm. "SRO" in Table 5 below means SrRuO3. The second intermediate layer of Example 8 was made of crystalline LaNiO3. The thickness of the second intermediate layer of Example 8 was 50 nm. "LNO" in Table 5 below means LaNiO3.

[0151] The thickness Ta of the first piezoelectric layer in each of Examples 7 and 8 was adjusted to the value shown in Table 6 below. The thickness Tb of the second piezoelectric layer in each of Examples 7 and 8 was adjusted to the value shown in Table 6 below. The thickness Tp of the piezoelectric thin film in each of Examples 7 and 8 was the value shown in Table 6 below.

[0152] Except for the above points, the piezoelectric thin film elements of Examples 7 and 8 were fabricated in the same manner as in Example 1.

[0153] The XRD patterns of the first electrode layers of Examples 7 and 8 were measured by the same method as in Example 1. In both Examples 7 and 8, the (002) plane of the Pt crystal constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.

[0154] The compositions of the piezoelectric thin films of Examples 7 and 8 were analyzed by the same method as in Example 1. In both Examples 7 and 8, the composition of the first piezoelectric layer was consistent with the composition of the first target, and the composition of the second piezoelectric layer was consistent with the composition of the second target.

[0155] The piezoelectric thin films of Examples 7 and 8 were analyzed using an X-ray diffractometer and STEM in the same manner as in Example 1. The piezoelectric thin films of Examples 7 and 8 had the following characteristics. The first piezoelectric layer was made of a perovskite-type tetragonal crystal 1. The second piezoelectric layer was made of a perovskite-type tetragonal crystal 2. The (001) plane of tetragonal crystal 1 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. The (001) plane of the tetragonal crystal 2 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. The c1 / a1 of the tetragonal crystal 1 in each of Examples 7 and 8 was the value shown in Table 6 below. The c2 / a2 of the tetragonal crystal 2 in each of Examples 7 and 8 was the value shown in Table 6 below. The I2 / (I1+I2) values ​​for Examples 7 and 8 were as shown in Table 6 below.

[0156] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin films of Examples 7 and 8 were evaluated. The Pr for each of Examples 7 and 8 is shown in Table 6 below. ε of Examples 7 and 8 r is shown in Table 6 below. -e of Examples 7 and 8 31,f is shown in Table 6 below. (-e 31,f ) 2 / ε0ε r is shown in Table 6 below.

[0157] [Table 5]

[0158] [Table 6]

[0159] Example 9 As shown in Table 7 below, the composition of the first target of Example 9 was the same as the composition of the first target of Example 1, and the composition of the second target of Example 9 was the same as the composition of the second target of Example 1.

[0160] In the process for producing the piezoelectric thin film element of Example 9, a first intermediate layer was not formed. In the process for producing the piezoelectric thin film element of Example 9, a first electrode layer made of crystalline SrRuO3 was formed directly on the entire surface of the single crystal substrate. The thickness of the first electrode layer of Example 9 was 200 nm.

[0161] The thickness Ta of the first piezoelectric layer of Example 9 was adjusted to the value shown in the following Table 8. The thickness Tb of the second piezoelectric layer of Example 9 was adjusted to the value shown in the following Table 8. The thickness Tp of the piezoelectric thin film of Example 9 was the value shown in the following Table 8.

[0162] The piezoelectric thin film element of Example 9 was produced in the same manner as in Example 1, except for the above points.

[0163] The XRD pattern of the first electrode layer of Example 9 was measured by the same method as in Example 1. The in-plane orientation of the crystals of the first electrode layer of Example 9 was evaluated by the same In-Plane measurement as in Example 1. In the case of Example 9, the crystal plane of the first electrode layer was not oriented in the in-plane direction of the surface of the first electrode layer. In other words, in the case of Example 9, the crystals of the first electrode layer did not have in-plane orientation.

[0164] The composition of the piezoelectric thin film of Example 9 was analyzed by the same method as in Example 1. In the case of Example 9, the composition of the first piezoelectric layer was consistent with the composition of the first target, and the composition of the second piezoelectric layer was consistent with the composition of the second target.

[0165] The piezoelectric thin film of Example 9 was analyzed using an X-ray diffractometer and STEM in the same manner as in Example 1. The piezoelectric thin film of Example 9 had the following characteristics. The first piezoelectric layer was made of a perovskite-type tetragonal crystal 1. The second piezoelectric layer was made of a perovskite-type tetragonal crystal 2. The (001) plane of tetragonal crystal 1 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. The (001) plane of the tetragonal crystal 2 was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. The c1 / a1 of the tetragonal crystal 1 of Example 9 was the value shown in Table 8 below. The c2 / a2 ratio of the tetragonal crystal 2 in Example 9 was the value shown in Table 8 below. The I2 / (I1+I2) values ​​in Example 9 were as shown in Table 8 below.

[0166] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin film of Example 9 were evaluated. Pr for Example 9 is shown in Table 8 below. ε in Example 9 r is shown in Table 8 below. Example 9-e 31,f is shown in Table 8 below. (-e 31,f ) 2 / ε0ε r is shown in Table 8 below.

[0167] [Table 7]

[0168] [Table 8] [Industrial Applicability]

[0169] A piezoelectric thin film according to one aspect of the present invention is applied to, for example, a piezoelectric transducer, a piezoelectric actuator, and a piezoelectric sensor. [Explanation of symbols]

[0170] 10...piezoelectric thin film element, 10a...ultrasonic transducer, 1...single crystal substrate, 2...first electrode layer, 3...piezoelectric thin film, 3A...first piezoelectric layer, 3B...second piezoelectric layer, 4...second electrode layer, 5...first intermediate layer, 6...second intermediate layer, D N ...normal direction to the surface of the single crystal substrate, dn...normal direction to the surface of the piezoelectric thin film, uc...unit cell of the perovskite structure, uc1...unit cell of tetragonal 1, uc2...unit cell of tetragonal 2.

Claims

1. 1. A piezoelectric thin film comprising a first piezoelectric layer and a second piezoelectric layer directly overlying the first piezoelectric layer, The first piezoelectric layer includes a tetragonal crystal 1 of a perovskite oxide, The second piezoelectric layer includes a tetragonal crystal 2 of a perovskite oxide, The (001) plane of the tetragonal crystal 1 is oriented in the normal direction to the surface of the piezoelectric thin film, The (001) plane of the tetragonal crystal 2 is oriented in the normal direction to the surface of the piezoelectric thin film, The spacing between the (001) planes of the tetragonal crystal 1 is c1, The spacing between the (100) planes of the tetragonal crystal 1 is a1, The spacing between the (001) planes of the tetragonal crystal 2 is c2, The spacing between the (100) planes of the tetragonal crystal 2 is a2, c2 / a2 is greater than c1 / a1, c1 / a1 is equal to or greater than 1.015 and equal to or less than 1.050, The peak intensity of the diffracted X-rays from the (001) plane of the tetragonal crystal 1 is I 1 , The peak intensity of the diffracted X-rays from the (001) plane of the tetragonal crystal 2 is I 2 ; I2 / (I1+I2) is equal to or greater than 0.91 and equal to or less than 0.99; The tetragonal crystal 1 is represented by the following chemical formula 1: In the following chemical formula 1, E A is at least one element selected from the group consisting of Na, K, and Ag; In the following chemical formula 1, E B is at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni, and Zn; In the following chemical formula 1, x1 is 0.10 or more and 0.90 or less, In the following chemical formula 1, y1 is 0.05 or more and 0.85 or less, In the following chemical formula 1, z1 is 0.05 or more and 0.85 or less, x1+y1+z1 is 1.00, In the following chemical formula 1, α is 0.00 or more and less than 1.00, The tetragonal crystal 2 is represented by the following chemical formula 2: In the following chemical formula 2, E A is at least one element selected from the group consisting of Na, K, and Ag; In the following chemical formula 2, E B is at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni, and Zn; In the following chemical formula 2, x2 is 0.10 or more and 0.85 or less, In the following chemical formula 2, y2 is 0.10 or more and 0.85 or less, In the following chemical formula 2, z2 is 0.05 or more and 0.80 or less, x2+y2+z2 is 1.00, In the following chemical formula 2, α is 0.00 or more and less than 1.

00. Piezoelectric thin film. x1(Bi 1-α E A α ) E B O 3 -y1BiFeO 3 -z1Bi(Fe 0.5 Ti 0.5 ) O 3 (1) x2(Bi 1-α E A α ) E B O 3 -y2BiFeO 3 -z2Bi(Fe 0.5 Ti 0.5 ) O 3 (2)

2. c2 / a2 is equal to or greater than 1.051 and equal to or less than 1.250; The piezoelectric thin film according to claim 1 .

3. The thickness of the first piezoelectric layer is 10 nm or more and 300 nm or less. The piezoelectric thin film according to claim 1 or 2.

4. A piezoelectric thin film according to any one of claims 1 to 3, Piezoelectric thin film element.

5. A single crystal substrate; an electrode layer overlying the single crystal substrate; the piezoelectric thin film overlying the electrode layer; Equipped with a first intermediate layer is disposed between the single crystal substrate and the electrode layer; The first intermediate layer is made of ZrO 2 and Y 2 O 3 Including, 5. The piezoelectric thin film element according to claim 4.

6. An electrode layer; the piezoelectric thin film overlying the electrode layer; Equipped with a second intermediate layer is disposed between the electrode layer and the piezoelectric thin film; The second intermediate layer is made of SrRuO 3 and LaNiO 3 At least one of the following is included:

6. The piezoelectric thin film element according to claim 4.

7. An electrode layer; the piezoelectric thin film overlying the electrode layer; Equipped with The electrode layer includes platinum crystals, the (002) plane of the platinum crystal is oriented in a direction normal to the surface of the electrode layer; The (200) plane of the platinum crystal is oriented in the in-plane direction of the surface of the electrode layer.

7. The piezoelectric thin film element according to claim 4.

8. A piezoelectric thin film element according to any one of claims 4 to 7, Piezoelectric transducer.

Citation Information

Patent Citations

  • Liquid drop jetting head, liquid drop jetting apparatus, and piezoelectric element

    JP2011093307A

  • JP2013‐191870A

  • Ceramic powder, piezoelectric ceramic, piezoelectric element, and electronic equipment

    JP2015180590A

  • Piezoelectric element and liquid discharge head

    JP2019114594A

  • Piezoelectric thin film, piezoelectric thin film element, piezoelectric actuator, piezoelectric sensor, head assembly, head stack assembly, hard disk drive, printer head, and inkjet printer device

    JP2020113649A