Resin, polycarbonate resin, and optical molding
A polycarbonate resin with high refractive index and transparency is produced by polymerizing a compound with a specific formula, addressing compatibility and thermal stability issues in existing resins, suitable for optical lenses and films.
Patent Information
- Application Number
- JP2023085672
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-28
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Existing polycarbonate resins have low refractive indices and blending sulfur-containing compounds to improve refractive index leads to decreased thermal stability and compatibility issues, affecting transparency.
A compound represented by a specific general formula is polymerized to produce a polycarbonate resin with high refractive index and excellent transparency, using a Suzuki-Miyaura coupling reaction and melt polycondensation method.
The resulting polycarbonate resin achieves a high refractive index and excellent transparency, suitable for optical molded articles such as lenses and films, with improved thermal stability and moldability.
Smart Images

Figure 0007588180000001 
Figure 0007588180000002 
Figure 0007588180000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound, a resin and a polycarbonate resin obtained from the compound, and an optical molded article containing the resin and the polycarbonate resin. [Background technology]
[0002] Optical glass or optical resin is used as a material for optical lenses used in the optical systems of various cameras such as cameras, film-integrated cameras, and video cameras. Optical glass is excellent in heat resistance, transparency, dimensional stability, chemical resistance, etc., and there are many types of materials with various refractive indices and Abbe numbers. However, there are problems such as high material costs, poor moldability, and low productivity.
[0003] On the other hand, optical lenses made of optical resins have the advantage that they can be mass-produced by injection molding. For example, polycarbonate resins are used in camera lenses. However, in recent years, the trend toward lighter, thinner, shorter and smaller products has led to a demand for the development of resins with higher refractive indices. In general, when the refractive index of an optical material is high, a lens element having the same refractive index can be realized with a surface with a smaller curvature, so that the amount of aberration generated by this surface can be reduced. As a result, it is possible to reduce the number of lenses, reduce the decentering sensitivity of the lens, and reduce the lens thickness to reduce its weight.
[0004] Techniques relating to optical resins include those described in Patent Documents 1 and 2, for example.
[0005] Patent Document 1 (JP-A-2005-241962) describes an optical lens made of a polycarbonate resin having a fluorene structure.
[0006] Patent Document 2 (JP-A-2005-187661) describes a method for easily improving the refractive index by blending (mixing, adding) a sulfur-containing compound with a fluorene-containing polyester. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-241962 A [Patent Document 2] JP 2005-187661 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the polycarbonate resin described in Patent Document 1 has a low refractive index and is not fully satisfactory. In addition, as described in Patent Document 2, blending a fluorene-containing polyester with a sulfur-containing compound improves the refractive index, but the thermal stability decreases due to the addition of a low molecular weight component, and transparency decreases if the compatibility of the two blended components is poor.
[0009] The present invention has been made in view of the above circumstances, and provides a resin and a polycarbonate resin that can realize an optical molded article having a high refractive index and excellent transparency. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to provide a polycarbonate resin capable of realizing an optically molded article having a high refractive index and excellent transparency. As a result, they have found that a resin obtained by polymerizing a compound represented by the following formula (1) can realize an optically molded article having a high refractive index and excellent transparency, and have arrived at the present invention.
[0011] According to the present invention, there are provided a compound represented by the following general formula (1), a resin obtained from the compound, a polycarbonate resin derived from the compound, and an optical molded article.
[0012] [1] A compound represented by general formula (1). [ka] (In general formula (1), Ar 1 and Ar 2 is, independently, [ka] R represents a group selected from 1 ~R 6 represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; A 1 ~A 5 and B. 1 ~B 5 represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; A 1 ~A 5 At least one of is -Y 1 -Ar 3 Group B 1 ~B 5 At least one of is -Y 2 -Ar 4 is a group, and Y 1 and Y 2 represents a single bond or a linking group, Ar 3 and Ar 4 represents an aromatic group, and X 1 ~X 4 is -O-, -S-, -NR'-, or -C(Me) 2 - and Z 1 ~Z 4 represents a hydrogen atom, a hydrocarbon group or a heteroatom-containing hydrocarbon group; R' represents a hydrogen atom, a hydrocarbon group or a heteroatom-containing hydrocarbon group; and o and p represent integers of 1 to 4). [2] The compound according to the above [1], wherein o and p in the above general formula (1) are 2. [3] Ar in the above general formula (1) 1 and Ar 2 is, independently, [ka] R represents a group selected from 1 ~R 6represents a hydrogen atom, a hydrocarbon group or a heteroatom-containing hydrocarbon group, and o and p represent integers of 1 to 4. The compound according to the above [1] or [2]. [4] A resin obtained by polymerizing a compound represented by general formula (1) according to any one of the above [1] to [3]. [5] A polycarbonate resin derived from a compound represented by general formula (1) according to any one of the above [1] to [3]. [6] An optically molded article comprising the resin according to [4] or [5] above. [7] The optical molded article according to the above [6], which is an optical lens. [8] The optical molded article according to the above [6], which is an optical film. Effect of the Invention
[0013] According to the present invention, it is possible to provide a resin and a polycarbonate resin that can realize an optical molded article having a high refractive index and excellent transparency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described. Note that unless otherwise specified, "~" between numbers in the text means "above" or "below."
[0015] [Compound] The compound according to this embodiment will be described below. The compound according to this embodiment is a compound represented by general formula (1). [ka] In general formula (1), Ar 1 and Ar 2 is, independently,
[0016] [ka] represents a group selected from R 1 ~R 6 represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; A1 ~A 5 and B. 1 ~B 5 represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; A 1 ~A 5 At least one of is -Y 1 -Ar 3 It is based on B 1 ~B 5 At least one of is -Y 2 -Ar 4 It is based on Y 1 and Y 2 represents a single bond or a linking group, Ar 3 and Ar 4 represents an aromatic group, and X 1 ~X 4 is -O-, -S-, -NR'-, or -C(Me) 2 - and Z 1 ~Z 4 represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; R' represents a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; o and p represent an integer of 1 to 4.
[0017] In the general formula (1), R 1 ~R 6 are each preferably independently selected from a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or an aryl group having 6 to 20 carbon atoms; R 1 ~R 6 are each more preferably independently selected from a hydrogen atom, a methyl group, a phenyl group, a biphenyl group, and a naphthyl group, and R 1 ~R 6 is more preferably a hydrogen atom.
[0018] In general formula (1), o and p are integers of 1 to 4, preferably 1 or 2, and more preferably 2. When o and p are within the above ranges, the polycarbonate resin obtained from the compound of general formula (1) has excellent heat resistance.
[0019] In one embodiment, Ar 1 and Ar 2 is, independently, [ka] R represents a group selected from 1 ~R 6 represents a hydrogen atom, a hydrocarbon group or a heteroatom-containing hydrocarbon group, and o and p represent integers of 1 to 4.
[0020] Ar in general formula (1) 1 and Ar 2 Preferred embodiments of the above include the following.
[0021] [ka]
[0022] [ka]
[0023] [ka]
[0024] Examples of the compound represented by the above general formula (1) include 9,9-bis(1'-hydroxymethyl)-2,7-dinaphthalene-2"-yl-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-dinaphthalene-1"-yl-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-3,6-dinaphthalene-2"-yl-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-3,6-dinaphthalene-1"-yl-9H-fluorene, and 9,9-bis(1'-hydroxymethyl)-2,7-di-p-biphenyl-9H-fluorene. fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-di-m-biphenyl-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis(3",5"-diphenylphenyl)-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis[dibenzo[b,d]thiophen-4"-yl]-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis(4"-phenoxy) phenyl)-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis(4"-phenylnaphthalen-1"-yl)-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis[4-(naphthalen-2-yl)phenyl]-9H-fluorene, 9,9-bis(1'-hydroxymethyl)-2,7-bis[3-naphthalen-2-yl]phenyl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)- 2,7-dinaphthalen-1"-yl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-3,6-dinaphthalen-2"-yl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-3,6-dinaphthalen-1"-yl-9H-naphthalene, 9,9-bis(2'-hydroxyethyl)-2,7-di-p-biphenyl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-di-m-biphenyl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-di-o-biphenyl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis(3",5"-diphenylphenyl)-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]thiophen-4"-yl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis(4"-phenoxyphenyl)-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis(3",5" -diphenoxyphenyl)-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis(4"-phenylnaphthalen-1"-yl)-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[4-(naphthalen-2-yl)phenyl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[3-(naphthalen-2-yl)phenyl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[3-(naphthalen-1-yl)phenyl]-9H-fluorene, 9 ,9-bis(2'-hydroxyethyl)-2,7-bis[4-(naphthalen-1-yl)phenyl]-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-diphenanthryl-9"-yl-9H-fluorene, 9,9-bis(2'-hydroxyethyl)-2,7-bis[9",9"-dimethyl-9"-fluoren-2"-yl]-9H-fluorene, 9,9-bis(3'-hydroxypropyl)-2,7-dinaphthalen-2"-yl-9H-fluorene, 9,9-bis(3'-hydroxypropyl)-2,7-dinaphthalene-1" -yl-9H-fluorene, 9,9-bis(3'-hydroxypropyl)-3,6-dinaphthalene-2"-yl-9H-fluorene, 9,9-bis(3'-hydroxypropyl)-3,6-dinaphthalene-1"-yl-9H-naphthalene, 9,9-bis(4'-hydroxybutyl)-2,7-dinaphthalene-2"-yl-9H-fluorene, 9,9-bis(4'-hydroxybutyl)-2,7-dinaphthalene-1"-yl-9H-fluorene, 9,9-bis(4'-hydroxybutyl)-3,6-dinaphthalene-2"-yl-9H-fluorene, 9,Examples include 9-bis(4'-hydroxybutyl)-3,6-dinaphthalen-1"-yl-9H-naphthalene, 9,9-bis(4'-hydroxybutyl)-3,6-bis[4-(naphthalen-2-yl)phenyl]-9H-fluorene, etc.
[0025] Of these, 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene and 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-1"-yl-9H-fluorene are preferable. These may be used alone or in combination of two or more.
[0026] [Method for producing the compound represented by formula (1)] The compound represented by general formula (1) of this embodiment can be synthesized by the following steps (i) and (ii). Step (i): A dihalogeno-9H-fluorene such as 2,7-dibromo-9H-fluorene or 3,6-dibromo-9H-fluorene is treated with a base (e.g., sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydride, potassium hydride, sodium methoxyl, sodium ethoxyl, sodium t-butoxyl, potassium t-butoxyl, n-butyllithium) in a solvent (e.g., tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, sulfolane). This abstracts the hydrogen at the 9-position of the dihalogeno-9H-fluorene, and then a hydroxyalkyl having a leaving group (examples of the leaving group include halogens such as chlorine, bromine, and iodine, p-toluenesulfonyloxy, methylsulfonyloxy, and trifluoromethylsulfonyloxy) is reacted to produce 9,9-bis(hydroxyalkyl)-dihalogeno-9H-fluorene such as 9,9-bis(hydroxyalkyl)-2,7-dibromo-9H-fluorene or 9,9-bis(hydroxyalkyl-3,6-9H-fluorene).
[0027] Step (ii): The 9,9-bis(hydroxyalkyl)-dihalogeno-9H-fluorene, such as 9,9-bis(hydroxyalkyl)-2,7-dibromo-9H-fluorene or 9,9-bis(hydroxyalkyl-3,6-9H-fluorene, obtained in step (i) is reacted with naphthylboric acid in a solvent (e.g., toluene and water, tetrahydrofuran and water, dimethylsulfoxide and water) in the presence of a base (e.g., sodium carbonate, potassium carbonate, sodium acetate, potassium acetate, sodium phosphate, potassium phosphate) and a palladium catalyst such as tetrakis(triphenylphosphine)palladium, to produce the target compound of general formula (1) under so-called Suzuki-Miyaura coupling conditions.
[0028] Here, the reaction in step (i) can be carried out at any temperature between −78° C. and the boiling point of the solvent. In addition, the reaction conditions can be those for general alkylation reactions. If desired, the hydroxy group of a hydroxyalkyl having a leaving group may be protected with any protecting group (for example, an ester group such as an acetyl group, an ether group such as a tetrahydropyranyl group, or a carbonate ester group such as a t-butoxycarbonyl group) and then finally deprotected.
[0029] The reaction in step (ii) can be carried out at any temperature between room temperature and the boiling point of the solvent, and the reaction conditions can be those generally used in the so-called Suzuki-Miyaura coupling.
[0030] [resin] One embodiment of the present invention is a resin obtained by polymerizing a compound represented by general formula (1). Examples of resins obtainable by polymerizing the compound represented by general formula (1) include polyester resins, polyurethane resins, polycarbonate resins, and polyether resins.
[0031] The polyester resin can be obtained by reacting the compound represented by general formula (1) with an aromatic dicarboxylic acid (e.g., terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid) or an aliphatic dicarboxylic acid (e.g., oxalic acid, malonic acid, succinic acid).
[0032] The polyurethane resin can be obtained by reacting the compound represented by general formula (1) with an aromatic diisocyanate (e.g., toluylene diisocyanate, xylylene diisocyanate) or an aliphatic diisocyanate (e.g., pentamethylene diisocyanate, hexamethylene diisocyanate, cyclohexanedimethylene diisocyanate).
[0033] As described later, the polycarbonate resin can be obtained by reacting a compound represented by the general formula (1) with a carbonate precursor such as a carbonic acid diester.
[0034] The polyether resin can be obtained by reacting the compound represented by general formula (1) with an aliphatic dihalogen compound (for example, dibromoethane, dibromopropane) in the presence of a base.
[0035] In these resins, reactants other than the compound represented by the general formula (1) of the present application may be used alone or in combination. It is also possible to polymerize the resin by using a dihydroxy compound other than the compound represented by the general formula (1) of the present application in combination.
[0036] When a dihydroxy compound other than the compound represented by general formula (1) of the present application is used in combination, the ratio of the compound represented by general formula (1) to the total of the compound represented by general formula (1) of the present application and the dihydroxy compound other than the compound represented by general formula (1) is preferably 5 mol % or more and 99 mol % or less, more preferably 10 mol % or more and 99 mol % or less, and even more preferably 15 mol % or more and 99 mol % or less.
[0037] Here, examples of dihydroxy compounds other than the compound represented by the general formula (1) include 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-ethylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-n-propylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-n-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-sec-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-tert-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-cyclohexylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-2-phenylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene, 9,9-bis[4-(2 -hydroxyethoxy)-3-(3-methylphenyl)phenyl]fluorene, bis[4-(2'-hydroxyethoxy)phenyl]sulfide, bis[4-(2'-hydroxyethoxy)-3-methylphenyl]sulfide, bis[4-(2'-hydroxyethoxy)phenyl]sulfone, bis[4-(2'-hydroxyethoxy)-3-methylphenyl]sulfone, bis[4-(2'-hydroxyethoxy)phenyl]sulfoxide, bis[4-(2'-hydroxyethoxy)phenyl]sulfoxide, bis(4-hydroxyphenyl)methane, 2 , 2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)phenylethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)heptane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 4,4-dihydroxyphenyl-1,1-m-diisopropylbenzene and other bis(4-hydroxyaryl)alkanes;Bis(hydroxyaryl)cycloalkanes such as 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and 2,2,2,2-tetrahydro-3,3,3,3-tetramethyl-1,1-spirobis〔1Hindene〕-6,6-diol; dihydroxyaryl ethers such as bis(4-hydroxyphenyl)ether and bis(4-hydroxy-3,5-dichlorophenyl)ether; 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydro 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene;ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 2,2-dimethyl-1,3-propanediol, 1,10-decanediol, diethylene glycol, tetraethylene glycol, norbornane dimethanol, decahydronaphthalene dimethanol, tricyclo[5.2.1.0; 2.6 ]Decanedimethanol, pentacyclopentadecanedimethanol, cyclopentane-1,3-dimethanol, spiroglycol, and the like can be mentioned.
[0038] [Polycarbonate resin] The polycarbonate resin according to this embodiment is produced using the compound represented by the general formula (1) according to this embodiment. The polycarbonate resin according to this embodiment has a structural unit derived from the compound represented by the general formula (1), which is represented by the formula (1p). Such a polycarbonate resin can realize an optical molded body having a high refractive index and excellent transparency. As a result, it can be suitably used as a material for optical lenses.
[0039] [ka]
[0040] In formula (1p), Ar 1 and Ar 2 , R 1 and R 2 and o and p have the same meanings as in formula (1). The same applies to preferred embodiments.
[0041] The polystyrene-equivalent weight average molecular weight (Mw) of the polycarbonate resin according to this embodiment is preferably 1.5×10 3 Above 2.0×10 5 More preferably, it is 2.0×10 or less. 3 More than 1.2 x 10 5 The following is the result.
[0042] It is preferable that Mw is equal to or greater than the lower limit, since it is possible to prevent the resulting molded body from becoming brittle.It is preferable that Mw is equal to or less than the upper limit, since it is possible to obtain a more appropriate melt viscosity, which makes it easier to remove the resin after production, and it is also possible to obtain a more satisfactory flowability, which makes it easier to perform injection molding in a molten state.
[0043] The refractive index (nD) of the polycarbonate resin according to this embodiment at 23° C. and a wavelength of 633 nm is preferably 1.70 or more and 1.85 or less, more preferably 1.70 or more and 1.82 or less, even more preferably 1.71 or more and 1.81 or less, and particularly preferably 1.72 or more and 1.81 or less.
[0044] The polycarbonate resin according to the present embodiment can be blended with other resins to produce a molded article. Examples of the other resins include polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polyethylene terephthalate, and polybutylene terephthalate.
[0045] Furthermore, the polycarbonate resin according to this embodiment may contain additives such as antioxidants, release agents, ultraviolet absorbers, flow modifiers, crystal nucleating agents, reinforcing agents, dyes, antistatic agents, and antibacterial agents.
[0046] Examples of molding methods include, in addition to injection molding, compression molding, casting, roll processing, extrusion molding, stretching, and the like, but are not limited to these.
[0047] When the polycarbonate resin according to this embodiment is used for injection molding, the preferred glass transition temperature (Tg) is 80°C or more and 190°C or less, more preferably 85°C or more and 180°C or less, and even more preferably 90°C or more and 170°C or less. When Tg is equal to or more than the lower limit, the temperature range of use is wider, which is preferable. When Tg is equal to or less than the upper limit, the melting temperature of the resin is lower, and decomposition or coloring of the resin is less likely to occur, which is preferable. When Tg is equal to or less than the upper limit, the difference between the mold temperature and the resin glass transition temperature can be reduced even with a general-purpose mold temperature regulator. Therefore, it is easy to use and preferable in applications where strict surface accuracy is required for the product.
[0048] The optically molded article obtained using the polycarbonate resin according to this embodiment has a total light transmittance, measured in accordance with JIS K-7361-1 (1997), of preferably 82% or more, more preferably 85% or more, which is comparable to that of bisphenol A-type polycarbonate resin and the like.
[0049] [Manufacturing method of polycarbonate resin] The polycarbonate resin according to the embodiment can be produced by using the compound represented by the above general formula (1) as a raw material. Specifically, the compound represented by the general formula (1) and a carbonate precursor such as a carbonic acid diester are reacted by a melt polycondensation method in the presence of a basic compound catalyst, an ester exchange catalyst, or a mixed catalyst consisting of both, or in the absence of a catalyst.
[0050] Examples of the carbonic acid diester used in the production of the polycarbonate resin according to the present embodiment include diphenyl carbonate, di-p-tolyl carbonate, di-m-tolyl carbonate, di-o-tolyl carbonate, bis(p-chlorophenyl) carbonate, bis(m-chlorophenyl) carbonate, bis(o-chlorophenyl) carbonate, m-cresyl carbonate, dimethyl carbonate, diethyl carbonate, di-n-butyl carbonate, and dicyclohexyl carbonate. Among these, diphenyl carbonate is preferred. Diphenyl carbonate is preferably used in a molar ratio of 0.97 to 1.20 with respect to 1 mole of the compound represented by general formula (1), and more preferably in a molar ratio of 0.98 to 1.10.
[0051] Examples of the basic compound catalyst used in the production of the polycarbonate resin according to the present embodiment include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds, etc. As such compounds, organic acid salts, inorganic salts, oxides, hydroxides, hydrides, or alkoxides of alkali metal and alkaline earth metal compounds, or quaternary ammonium hydroxides and their salts, amines, etc. are preferably used, and these compounds can be used alone or in combination.
[0052] Examples of the alkali metal compound include organic acid salts, inorganic salts, oxides, hydroxides, hydrides, and alkoxides of alkali metals.Specific examples include sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium hydrogen carbonate, sodium carbonate, potassium hydrogen carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium phenyl borohydride, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenyl phosphate, disodium salt, dipotassium salt, dicesium salt, or dilithium salt of bisphenol A, and sodium salt, potassium salt, cesium salt, or lithium salt of phenol.
[0053] Examples of the alkaline earth metal compound include organic acid salts, inorganic salts, oxides, hydroxides, hydrides, and alkoxides of alkaline earth metal compounds.Specific examples include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium hydrogen carbonate, calcium hydrogen carbonate, strontium hydrogen carbonate, barium hydrogen carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium acetate, calcium acetate, strontium acetate, barium acetate, magnesium stearate, calcium stearate, calcium benzoate, and magnesium phenylphosphate.
[0054] Examples of the nitrogen-containing compound include quaternary ammonium hydroxides and their salts, amines, etc. Specifically, quaternary ammonium hydroxides having an alkyl group, an aryl group, etc., such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetra-n-propylammonium hydroxide, tetra-n-butylammonium hydroxide, and trimethylbenzylammonium hydroxide; tertiary amines such as triethylamine, dimethylbenzylamine, and triphenylamine; secondary amines such as diethylamine and dibutylamine; primary amines such as n-propylamine and n-butylamine; imidazoles such as 2-methylimidazole, 2-phenylimidazole, and benzimidazole; or bases or basic salts such as ammonia, tetramethylammonium borohydride, tetra-n-butylammonium borohydride, tetra-n-butylammonium tetraphenylborate, and tetraphenylammonium tetraphenylborate, etc., are used.
[0055] As the transesterification catalyst, a salt of zinc, tin, zirconium, lead, etc. is preferably used, and these can be used alone or in combination. Specific examples of the transesterification catalyst include zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin chloride (II), tin chloride (IV), tin acetate (II), tin acetate (IV), dibutyltin dilaurate, dibutyltin oxide, dibutyltin dimethoxide, zirconium acetylacetonate, zirconium oxyacetate, zirconium tetrabutoxide, lead acetate (II), lead acetate (IV), etc. These catalysts are used in an amount of 10 -9 ~10 -3 In terms of molar ratio, preferably 10 -7 ~10 -4 Used in molar ratios.
[0056] The melt polycondensation method uses the above-mentioned raw materials and catalyst and carries out melt polycondensation under heating at normal pressure or reduced pressure while removing by-products through an ester exchange reaction. In the melt polycondensation method according to this embodiment, it is desirable to melt the compound represented by the above general formula (1) and the carbonate diester in a reaction vessel, and then carry out the reaction while retaining the by-produced monohydroxy compound.
[0057] In order to retain the reaction mixture, the pressure can be controlled by blocking the reaction apparatus, reducing or increasing the pressure, etc. The reaction time in this step is preferably 20 minutes or more and 240 minutes or less, more preferably 40 minutes or more and 180 minutes or less, and particularly preferably 60 minutes or more and 150 minutes or less. In this case, if the by-product monohydroxy compound is distilled off immediately after production, the polycarbonate resin finally obtained has a low content of high molecular weight compounds. However, if the by-product monohydroxy compound is retained in the reaction vessel for a certain period of time, the polycarbonate resin finally obtained has a high content of high molecular weight compounds.
[0058] Generally, the melt polycondensation reaction is carried out in a multi-stage process of two or more stages. Specifically, the first stage reaction is carried out at a temperature of preferably 120 to 260°C, more preferably 180 to 240°C, under normal pressure or pressure, for preferably 0.1 to 5 hours, more preferably 0.5 to 3 hours. Next, the reaction temperature is increased while increasing the degree of vacuum of the reaction system to react the compound represented by general formula (1) with the carbonate diester, and finally, the polycondensation reaction is preferably carried out at a degree of vacuum of 133 Pa (1 mmHg) or less and a temperature of 200 to 350°C for 0.05 to 2 hours.
[0059] The melt polycondensation reaction may be carried out in a continuous manner or in a batch manner. The reaction apparatus used for carrying out the reaction may be a vertical type equipped with an anchor-type impeller, a Maxblend impeller, a helical ribbon-type impeller, etc., a horizontal type equipped with a paddle impeller, a lattice impeller, a spectacle impeller, etc., or an extruder type equipped with a screw. In addition, it is preferable to use a reaction apparatus that is an appropriate combination of these reaction apparatuses, taking into consideration the viscosity of the polymer.
[0060] After the polycondensation reaction is completed, the polycarbonate resin according to the present embodiment may have the catalyst removed or deactivated in order to maintain thermal stability and hydrolysis stability. In general, a method of deactivating the catalyst by adding a known acidic substance can be suitably carried out. Specific examples of the acidic substance include esters such as butyl benzoate; aromatic sulfonic acids such as p-toluenesulfonic acid; aromatic sulfonic acid esters such as butyl p-toluenesulfonate and hexyl p-toluenesulfonate; phosphoric acids such as phosphorous acid, phosphoric acid, and phosphonic acid; phosphite esters such as triphenyl phosphite, monophenyl phosphite, diphenyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-n-butyl phosphite, di-n-hexyl phosphite, di-n-octyl phosphite, and mono-n-octyl phosphite; triphenyl phosphate, diphenyl phosphate, monophenyl phosphate, di-n-butyl phosphate, and di-n-octyl phosphate. Phosphates such as mono-n-octyl phosphate; phosphonic acids such as diphenylphosphonic acid, di-n-octylphosphonic acid, di-n-butylphosphonic acid; phosphonic acid esters such as diethyl phenylphosphonate; phosphines such as triphenylphosphine and bis(diphenylphosphino)ethane; boric acid and phenylboric acid; aromatic sulfonates such as tetra-n-butylphosphonium n-dodecylbenzenesulfonate; organic halides such as stearic acid chloride, benzoyl chloride, and p-toluenesulfonic acid chloride; alkyl sulfates such as dimethyl sulfate; organic halides such as benzyl chloride, and the like are preferably used. These deactivators are preferably used in an amount of 0.01 to 50 times by mole, more preferably 0.3 to 20 times by mole, based on the amount of the catalyst. If the amount is less than 0.01 times by mole based on the amount of the catalyst, the deactivation effect is insufficient, which is not preferable. If the amount is more than 50 times by mole based on the amount of the catalyst, the heat resistance of the resin decreases and the molded body is easily colored, which is not preferable.
[0061] After the catalyst is deactivated, a step may be provided in which low-boiling compounds in the polymer are removed by volatilization at a pressure of 13 to 133 Pa (0.1 to 1 mmHg) and a temperature of 200 to 350° C. In this step, a horizontal apparatus equipped with stirring blades with excellent surface renewal ability, such as paddle blades, lattice blades, and spectacle blades, or a thin-film evaporator is preferably used.
[0062] The polycarbonate resin according to the present embodiment is desired to have a minimum foreign matter content, and filtration of the molten raw material, filtration of the catalyst solution, etc. are preferably carried out. The mesh of the filter is preferably 5 μm or less, more preferably 1 μm or less. Furthermore, filtration of the produced resin with a polymer filter is preferably carried out. The mesh of the polymer filter is preferably 100 μm or less, more preferably 30 μm or less. Furthermore, the process of collecting the resin pellets is naturally preferably carried out in a low dust environment, and more preferably has a cleanliness level of class 1000 or less.
[0063] [Optical molded object] The optical molded article according to this embodiment contains the polycarbonate resin according to this embodiment, and the optical molded article can be produced using the polycarbonate resin according to this embodiment. For example, the molding may be performed by any method such as injection molding, compression molding, injection compression molding, extrusion molding, solution casting, or the like. The polycarbonate resin according to the present embodiment has excellent moldability and heat resistance, and can be used particularly advantageously in optical lenses that require injection molding. During molding, the polycarbonate resin according to the present embodiment can be mixed with other resins such as other polycarbonate resins and polyester resins.
[0064] In addition, various additives can be used to impart various properties to the extent that the object of this embodiment is not impaired. Examples of additives include antioxidants, processing stabilizers, release agents, ultraviolet absorbers, bluing agents, polymerized metal deactivators, flame retardants, lubricants, antistatic agents, heat shielding agents, fluorescent dyes (including fluorescent brighteners), pigments, light scattering agents, reinforcing fillers, surfactants, antibacterial agents, plasticizers, compatibilizers, other resins and elastomers, etc.
[0065] Examples of the antioxidant include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, t-butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. The content of the antioxidant in the polycarbonate resin is preferably 0.001 to 0.3 parts by mass with respect to 100 parts by mass of the polycarbonate resin.
[0066] Examples of the processing stabilizer include phosphorus-based processing heat stabilizers and sulfur-based processing heat stabilizers.
[0067] Examples of phosphorus-based heat-treatment stabilizers include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof. Specific examples include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, tri-n-decyl phosphite, tri-n-octyl phosphite, tri-n-octadecyl phosphite, di-n-decyl monophenyl phosphite, di-n-octyl monophenyl phosphite, diisopropyl monophenyl phosphite, mono-n-butyl diphenyl phosphite, and the like. phenyl phosphite, monodecyl diphenyl phosphite, mono n-octyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl) octyl phosphite, bis(n-nonylphenyl) pentaerythritol diphosphite, bis(2,4-dicumylphenyl) pentaerythritol diphosphite, bis(2,4-di-tert -butylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tri-n-butyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl monoorthoxenyl phosphate, di-n-butyl phosphate, di-n-octyl phosphate, diisopropyl phosphate, dimethyl benzenephosphonate, diethyl benzenephosphonate, dipropyl benzenephosphonate, tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-t-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,4-di-t-butylphenyl)-3,3'-biphenylene diphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphonite and bis(2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphonite. The content of the phosphorus-based processing heat stabilizer in the polycarbonate resin is preferably 0.001 to 0.2 parts by mass with respect to 100 parts by mass of the polycarbonate resin.
[0068] Examples of sulfur-based processing heat stabilizers include pentaerythritol-tetrakis(3-laurylthiopropionate), pentaerythritol-tetrakis(3-myristylthiopropionate), pentaerythritol-tetrakis(3-stearylthiopropionate), dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, and distearyl-3,3'-thiodipropionate. The content of the sulfur-based processing heat stabilizer in the polycarbonate resin is preferably 0.001 to 0.2 parts by mass with respect to 100 parts by mass of the polycarbonate resin.
[0069] The release agent is preferably one that is composed of 90% by mass or more of an ester of alcohol and fatty acid. Specific examples of the ester of alcohol and fatty acid include an ester of monohydric alcohol and fatty acid, and a partial ester or full ester of polyhydric alcohol and fatty acid. The ester of monohydric alcohol and fatty acid is preferably an ester of monohydric alcohol having 1 to 20 carbon atoms and saturated fatty acid having 10 to 30 carbon atoms. In addition, the partial ester or full ester of polyhydric alcohol and fatty acid is preferably a partial ester or full ester of polyhydric alcohol having 1 to 25 carbon atoms and saturated fatty acid having 10 to 30 carbon atoms.
[0070] Examples of esters of monohydric alcohols and saturated fatty acids include stearyl stearate, palmityl palmitate, n-butyl stearate, methyl laurate, isopropyl palmitate, etc. Examples of partial or full esters of polyhydric alcohols and saturated fatty acids include full or partial esters of dipentaerythritol, such as stearic acid monoglyceride, stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearic acid monosorbitate, behenic acid monoglyceride, capric acid monoglyceride, lauric acid monoglyceride, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, biphenyl biphenate, sorbitan monostearate, 2-ethylhexyl stearate, and dipentaerythritol hexastearate.
[0071] The content of these release agents is preferably in the range of 0.005 to 2.0 parts by mass, more preferably in the range of 0.01 to 0.6 parts by mass, and further preferably in the range of 0.02 to 0.5 parts by mass, relative to 100 parts by mass of the polycarbonate resin.
[0072] The ultraviolet absorber is preferably at least one ultraviolet absorber selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, cyclic iminoester ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers. The ultraviolet absorbers listed below may be used alone or in combination of two or more.
[0073] Examples of the benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butyl phenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-n-octyloxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, and the like.
[0074] Examples of benzophenone-based ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridolate benzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.
[0075] Examples of triazine-based ultraviolet absorbers include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(n-hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-[(n-octyl)oxy]-phenol.
[0076] Examples of cyclic imino ester-based ultraviolet absorbers include 2,2'-bis(3,1-benzoxazine-4-one), 2,2'-p-phenylenebis(3,1-benzoxazine-4-one), 2,2'-m-phenylenebis(3,1-benzoxazine-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzoxazine-4-one), 2,2'-(2,6-naphthalene)bis(3,1-benzoxazine-4-one), 2,2'-(1,5-naphthalene)bis(3,1-benzoxazin-4-one), 2,2'-(2-methyl-p-phenylene)bis(3,1-benzoxazin-4-one), 2,2'-(2-nitro-p-phenylene)bis(3,1-benzoxazin-4-one), and 2,2'-(2-chloro-p-phenylene)bis(3,1-benzoxazin-4-one).
[0077] Examples of cyanoacrylate ultraviolet absorbers include 1,3-bis-[(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.
[0078] The content of the ultraviolet absorber is preferably 0.01 to 3.0 parts by mass, more preferably 0.02 to 1.0 parts by mass, and further preferably 0.05 to 0.8 parts by mass, relative to 100 parts by mass of the polycarbonate resin. If the blending amount is within this range, it is possible to impart sufficient weather resistance to the polycarbonate resin depending on the application.
[0079] Examples of bluing agents include Macrolex Violet B and Macrolex Blue RR from Bayer, and Polysynthren Blue RLS from Clariant.
[0080] Bluing agents are effective in removing the yellowish tinge of polycarbonate resin. In particular, in the case of weather-resistant polycarbonate resin, a certain amount of ultraviolet absorbing agent is blended, and the polycarbonate resin molded product tends to have a yellowish tinge due to the "action and color of the ultraviolet absorbing agent", so blending a bluing agent is particularly effective in imparting a natural transparency to sheets and lenses. The blending amount of the bluing agent is, for example, preferably 0.05 to 1.5 ppm, and more preferably 0.1 to 1.2 ppm, relative to the polycarbonate resin.
[0081] The polycarbonate resin according to the present embodiment exhibits a high refractive index and excellent heat resistance, and has a flowability suitable for molding.Furthermore, since it has low birefringence and is unlikely to cause optical distortion, it can be advantageously used as an optical molded body suitable for structural or functional materials for optical components such as transparent conductive substrates used in liquid crystal displays, organic EL displays, solar cells, optical disks, liquid crystal panels, optical cards, sheets, films, optical fibers, connectors, evaporated plastic reflectors, and displays, in addition to optical lenses.
[0082] The surface of the optical molded body may be provided with a coating layer such as an anti-reflection layer or a hard coat layer as necessary. The anti-reflection layer may be a single layer or a multilayer, and may be an organic or inorganic material, but is preferably an inorganic material. Specific examples of the anti-reflection layer include oxides or fluorides such as silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, cerium oxide, magnesium oxide, and magnesium fluoride.
[0083] (Optical Lenses) The optical lens manufactured using the polycarbonate resin according to the present embodiment has a high refractive index and excellent heat resistance, and can be used in fields where expensive high refractive index glass lenses have been used in the past, such as telescopes, binoculars, and television projectors, and is extremely useful. It is preferable to use it in the form of an aspherical lens as necessary. Since an aspherical lens can substantially reduce spherical aberration with one lens, it is not necessary to remove spherical aberration by combining multiple spherical lenses, and it is possible to reduce weight and production costs. Therefore, the aspherical lens is particularly useful as a camera lens among optical lenses. The optical lens according to this embodiment is molded by any method, such as injection molding, compression molding, injection compression molding, etc. According to this embodiment, it is possible to more easily obtain a high refractive index, low birefringence aspheric lens, which is technically difficult to process using glass lenses.
[0084] (Optical film) The optical film produced using the polycarbonate resin according to this embodiment has excellent transparency and heat resistance, and is therefore suitable for use as a film for liquid crystal substrates, optical memory cards, and the like.
[0085] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES
[0086] The present embodiment will be described in detail below with reference to examples and comparative examples, but the present embodiment is not limited to the descriptions of these examples.
[0087] 1. Measurement and evaluation methods In the following Examples and Comparative Examples, the measurements and evaluations of the various physical properties were carried out by the following methods.
[0088] 1) Weight average molecular weight (Mw) in terms of polystyrene: A calibration curve was prepared using a gel permeation chromatograph (GPC: Waters 1515, 2414 and 2489) with chloroform as the eluent and standard polystyrene of known molecular weight (molecular weight distribution = 1). Based on this calibration curve, Mw was calculated from the GPC retention time.
[0089] 2) Refractive index (n633): A chloroform solution of 8.5 wt% resin was coated on a silicon wafer using a spin coater at 200 rpm for 20 seconds and 1000 rpm for 5 seconds, and then baked at 120°C for 5 minutes and 200°C for 2 minutes to prepare a sample. The refractive index and film thickness of the film were calculated by fitting the following optical model to the optical measurement data at wavelengths of 200-1000 nm using a spectroscopic ellipsometer GES5E (manufactured by SEMILAB). (Optical model) Laminated structure: Film / SiO 2 (2nm thickness) / Si substrate (500μm thickness) Dispersion equation of film: Cauchy + Lorentz oscillator model
[0090] 3) Glass transition temperature (Tg): Measured with a differential scanning calorimeter (DSC: Shimadzu Corporation DSC-60).
[0091] 1. Preparation of the compound represented by formula (1) Example 1 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene Step (i): Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-dibromo-9H-fluorene 66.5g (0.2mol) of 2,7-dibromo-9H-fluorene, 56g (0.998mol) of potassium hydroxide (powder), 3.4g (0.02mol) of potassium iodide, and 150ml of dimethyl sulfoxide were charged into a 500ml flask and cooled to 10°C with ice water. Then, 58.4g (0.467mol) of 2-bromoethanol was added dropwise over 45 minutes, and the mixture was stirred at room temperature overnight. The reaction solution was then heated to 50°C and stirred for 40 hours. The reaction mixture was poured into 2L of distilled water, and the pH was adjusted to 6 with concentrated hydrochloric acid. The solid obtained was filtered and washed with 3L of water. The obtained solid was dissolved in 1 liter of ethyl acetate, washed with 500 ml of distilled water, concentrated using an evaporator, and added with chloroform to obtain 34.8 g of 9,9-bis(2'-hydroxyethyl)-2,7-dibromo-9H-fluorene as colorless crystals.
[0092] Step (ii): Preparation of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene A 1-liter flask was charged with 20.75 g (50 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dibromo-9H-fluorene, 19.17 g (0.11 mol) of naphthalene-2-boronic acid, 15.3 g (0.11 mol) of potassium carbonate, 250 g of distilled water, and 400 g of dimethyl sulfoxide. 3.0 g of tetrakis(triphenylphosphine)palladium was added to this reaction mixture, which was then heated to 100°C and stirred for 5 hours. After cooling, the resulting solid was filtered off, washed with 500 g of water, and vacuum dried at 50°C. After drying, the solid was suspended and washed in chloroform to obtain 20.87 g of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalene-2"-yl-9H-fluorene as colorless crystals. The melting point measured by DSC was 236°C.
[0093] Example 2 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene Step (i): Synthesis of 2-(2'-bromoethoxy)tetrahydropyran A 2-liter round-bottom flask equipped with a stirrer, a thermometer, and a dropping funnel was charged with 150 g (1.20 mol) of 2-bromoethanol and 800 ml of dichloromethane, and cooled with ice water. Then, when the internal temperature reached 5°C, 130 g (1.56 mol) of 3,4-dihydro-2H-pyran was added dropwise at 10°C or less. After the dropwise addition, 30 g (0.12 mol) of pyridinium p-toluenesulfonate was added, and the mixture was stirred at room temperature overnight. Then, saturated water with sodium bicarbonate was added, and the dichloromethane layer was washed with water. The obtained dichloromethane layer was concentrated with an evaporator to obtain 255 g of 2-(2'-bromoethoxy)tetrahydropyran as a pale yellow oil.
[0094] Step (ii): Synthesis of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dibromo-9H-fluorene 255g of 2-(2'-bromoethoxy)tetrahydropyran, 270ml of toluene, and 164g (0.506mol) of 2,7-dibromo-9H-fluorene were charged in a 2-liter round-bottom flask equipped with a stirrer, a thermometer, and a reflux condenser, and 270ml of 50% aqueous sodium hydroxide solution was added thereto. Then, 8.5g (26.2mmol) of tetrabutylammonium bromide was added, and the mixture was heated to 100°C and stirred for 11.5 hours. Then, the reaction mixture was cooled to room temperature, and the aqueous layer was separated, and then 700ml of ethyl acetate and 700ml of distilled water were added, followed by washing with water. After repeated washing with water, the layer consisting of ethyl acetate and toluene was separated and concentrated with an evaporator. A small amount of seed crystals of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dibromo-9H-fluorene was added to the viscous liquid obtained after concentration, and crystallization was performed by adding methanol. The resulting crystals were filtered, washed with a small amount of methanol, and then recrystallized by heating from 500 ml of methanol to obtain 246 g of the desired 9,9-bis[2-(2'-tetrahydropyranyl)ethoxy]-2,7-dibromo-9H-fluorene as pale yellow crystals. mp98.5℃ 1 H-NMR (CDCl 3) δ1.30-1.53(m,12H), 2.34-2.38(t,4H), 2.70-3.5(m, 8H), 4.1(t, 2H), 7.43-7.55(m, 6H)
[0095] Step (iii): Synthesis of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene 72.55g (125mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dibromo-9H-fluorene, 475ml of toluene, 61g (442mmol) of potassium carbonate, 47.29g (275mmol) of 2-naphthaleneboronic acid, and 211ml of distilled water were charged into a 1-liter round-bottom flask equipped with a stirrer, a thermometer, and a reflux condenser, and 1.4g of tetrakis(triphenylphosphine)palladium was added to the reaction mixture while stirring, and the temperature was raised to 80°C. The mixture was heated and stirred at 80°C for 12 hours, and then cooled to room temperature. After separating the aqueous layer, the toluene layer was washed with distilled water, and then the toluene layer was concentrated by an evaporator. 730ml of methanol was added to the concentrated residue, and the resulting solid was filtered and washed with methanol. The product was then purified by silica gel column chromatography (eluent: toluene to toluene / ethyl acetate = 9 / 1), and then recrystallized from methyl cellosolve to obtain 121.01 g of the target product. Yield: 72%, HPLC purity: 99.3%, mp: 148°C, 1 H-NMR (CDCl 3 ) δ1.20-1.70(m, 12H), 2,55(t, 4H), 2.8-3.5(m, 8H), 4.16(m,2H), 7.40-7.65(m, 4H), 7.70-8.05(m, 14H), 8.1(s, 2H)
[0096] Step (iv): Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene In a 1-liter round-bottom flask equipped with a stirrer, a thermometer, and a reflux condenser, 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water, and 7 ml of concentrated hydrochloric acid were charged, and the mixture was heated to 115°C with stirring and stirred at the same temperature for 4 hours. After that, the mixture was cooled to room temperature, 180 ml of water was added, and the resulting crystals were filtered off. The obtained crystals were washed with distilled water, dried under reduced pressure at 50°C, and then suspended and washed with hot methyl cellosolve to obtain 38.73 g of the target product. Yield 85%, mp 249.5°C, 1 H-NMR (DMSO-d 6 ) δ2.43(t, 4H), 2.80(t, 4H), 4.16(t, 2H), 7.50-7.60(m,4H), 7.8-8.1(m,12H), 8.35(s,2H)
[0097] Example 3 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4”-yl]-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 58.85 g (275 mmol) of dibenzo[b,d]furan-4-ylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 66.05 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene. Yield: 70%, HPLC purity: 97.5%, MP: 176.7°C. 1 H-NMR (CDCl 3) δ1.29-1.45 (10H, m), 1.58 (2H, m), 2.58 (4H, t), 2.98 (2H, q), 3.24 (2H, dt), 3.40 (2H, q), 3.55 (2H, dt), 4.23 (2H, s), 7.39 (2H, t), 7.48 (4H, q), 7.64 (2H, d), 7.68-7.71 (2H, m), 7.90-8.03 (10H, m)
[0098] The procedure described in step (iv) of Example 2 was followed except that 60.00 g (79.4 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene, 540 ml of methyl cellosolve, 22 ml of distilled water and 6.2 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 41.03 g of the target product. Yield: 88%, HPLC purity: 99.4%, MP: 247.4°C. 1 H-NMR (DMSO-d 6 ) δ2.40 (4H, t), 2.98 (4H, m), 4.24 (2H, t), 7.46 (2H, t), 7.58 (4H, dt), 7.82 (4H, dd), 8.03-8.10 (6H, m), 8.22 (4H, dd)
[0099] Example 4 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis〔4-(naphthalen-2-yl)phenyl〕-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 68.22 g (275 mmol) of 4-(naphthalene-2-yl)phenylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 68.23 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4-(naphthalene-2-yl)phenyl]-9H-fluorene. Yield 66%, HPLC purity 99.2%, MP 209.4°C. 1 H-NMR (CDCl 3 ) δ1.26-1.61 (12H, m), 2.55 (4H, t), 2.86 (2H, q), 3.22-3.32 (4H, m), 3.51-3.56 (2H, m), 4.17 (2H, t), 7.49-7.55 (4H, m), 7.67 (2H, d), 7.75 (2H, d), 7.78-7.82 (6H, m), 7.84-7.90 (8H, m), 7.95 (4H, t), 8.13 (2H, s)
[0100] The procedure described in step (iv) of Example 2 was followed except that 60.00 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4-(naphthalen-2-yl)phenyl]-9H-fluorene, 500 ml of methyl cellosolve, 20 ml of distilled water and 6 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 41.10 g of the target product. Yield: 86%, HPLC purity: 99.6%, MP3: 41.3°C. 1 H-NMR (DMSO-d 6) δ2.41 (4H, t), 2.83 (4H, q), 4.20 (2H, t), 7.53-7.60 (4H, m), 7.83 (2H, d), 7.94-8.00 (16H, m), 8.06 (4H, d), 8.33 (2H, s)
[0101] Example 5 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis〔3-(naphthalen-2-yl)phenyl〕-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 68.22 g (275 mmol) of 3-(naphthalen-2-yl)phenylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2, to obtain 70.30 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[3-(naphthalen-2-yl)phenyl]-9H-fluorene. Yield 68%, HPLC purity 98.9%, MP 171.6°C. 1 H-NMR (CDCl 3 ) δ1.26-1.58 (12H, m), 2.54 (4H, t), 2.86 (2H, q), 3.22-3.30 (4H, m), 3.49-3.54 (2H, m), 4.16 (2H, t), 7.51-7.61 (6H, m), 7.66-7.74 (8H, m), 7.81 (2H, d), 7.84 (2H, dd), 7.90 (2H, d), 7.94-7.99 (6H, m), 8.14 (2H, s)
[0102] In step (iv) of Example 2, instead of using 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[3-(naphthalen-2-yl-)fluorene] was used. The procedure described in step (iv) of Example 2 was followed except that 60.00 g (72.5 mmol) of [phenyl]-9H-fluorene, 500 ml of methyl cellosolve, 20 ml of distilled water, and 5.7 g of concentrated hydrochloric acid were used to obtain 41.58 g of the target product. Yield: 87%. The final product was purified by column chromatography (eluent: ethyl acetate / chloroform = 1 / 8 → 1 / 4). HPLC purity: 99.7%, mp: 143.1°C. 1 H-NMR (DMSO-d 6 ) δ: 2.52 (4H, t), 3.17 (4H, q), 7.51-7.54 (4H, m), 7.60 (2H, t), 7.67-7.69 (2H, m), 7.74 (2H, dd), 7.76 (2H, s), 7.82-7.91 (6H, m), 7.94-7.99 (6H, m), 8.14 (2H, s)
[0103] Example 6 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-diphenanthren-9"-yl-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 61.06 g (275 mmol) of phenanthren-9-ylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 73.62 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-diphenanthren-9"-yl-9H-fluorene. Yield: 76%, HPLC purity: 95.9%, viscous solid. 1 H-NMR (CDCl 3) δ1.36-1.64 (12H, m), 2.50 (4H, t), 2.99 (2H, q), 3.30-3.43 (4H, m), 3.58 (2H, dt), 4.29 (2H, s), 7.57 (4H, d), 7.63-7.72 (8H, m), 7.77 (2H, s), 7.90 (2H, d), 7.93-7.95 (2H, m), 8.03 (2H, d), 8.79 (4H, dd)
[0104] In step (iv) of Example 2, 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene 60.00 g (88.9 mmol), 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid were used instead of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-diphenanthren-9"-yl-9H-fluorene 70.00 g (90.3 mmol), 610 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid were used in place of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene 60.00 g (88.9 mmol), 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, and the procedure described in step (iv) of Example 2 was followed to obtain 48.22 g of the target product. Yield: 88%. The final product was purified by column chromatography (eluent: ethyl acetate / chloroform = 1 / 6 ⇒ 1 / 4). HPLC purity: 99.3%, mp 226.9°C, 1 H-NMR (DMSO-d 6 ) δ2.48 (4H, t), 3.31 (4H, q), 7.57-7.73 (12H, m), 7.77 (2H, s), 7.95 (6H, dd), 8.79 (4H, dd)
[0105] Example 7 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]thiophen-4”-yl]-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 62.72 g (275 mmol) of dibenzo[b,d]thiophen-4-ylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 68.87 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[dibenzo[b,d]thiophen-4"-yl]-9H-fluorene. Yield: 70%, HPLC purity: 99.1%, viscous solid. 1 H-NMR (CDCl 3 ) δ1.28-1.43 (10H, m), 1.55 (2H, m), 2.56 (4H, t), 2.95 (2H, q), 3.22 (2H, dt), 3.37 (2H, q), 3.52 (2H, dt), 4.20 (2H, s), 7.51 (2H, t), 7.68 (4H, q), 7.85 (2H, d), 7.82-7.89 (2H, m), 8.11-8.24 (10H, m)
[0106] The procedure described in step (iv) of Example 2 was followed except that 60.00 g (76.4 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[dibenzo[b,d]thiophen-4"-yl]-9H-fluorene, 500 ml of methyl cellosolve, 20 ml of distilled water and 6.0 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 40.10 g of the target product. Yield 85%, HPLC purity 98.9%, MP2 23.6°C. 1 H-NMR (DMSO-d 6) δ2.38 (4H, t), 2.93 (4H, dt), 4.26 (2H, t), 7.57 (4H, dd), 7.69-7.71 (4H, m), 7.79 (2H, d), 7.97 (2H, s), 8.04 (2H, dd), 8.10 (2H, d), 8.43-8.47 (4H, dd)
[0107] Example 8 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis〔4"-phenoxyphenyl〕-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 58.86 g (275 mmol) of 4-phenoxyphenylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2, to obtain 68.31 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4-phenoxyphenyl]-9H-fluorene. Yield 72%, HPLC purity 98.8%, viscous solid. 1 H-NMR (CDCl 3 ) δ1.24-1.59 (12H, m), 2.48 (4H, t), 2.81 (2H, q), 3.20-3.27 (4H, m), 3.48-3.54 (2H, m), 4.14 (2H, t), 7.07-7.15 (10H, m), 7.37 (4H, dt), 7.55 (2H, d), 7.60-7.63 (6H, m), 7.74 (2H, d)
[0108] The procedure described in step (iv) of Example 2 was followed except that 60.00 g (79.1 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4"-phenoxyphenyl]-9H-fluorene, 530 ml of methyl cellosolve, 22 ml of distilled water and 6.2 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 38.29 g of the target product. Yield: 82%, HPLC purity: 99.7%, MP: 134.1°C. 1 H-NMR (DMSO-d 6 ) δ2.34 (4H, t), 2.76 (4H, q), 4.14 (2H, t), 7.07-7.20 (10H, m), 7.43 (4H, t), 7.67 (2H, dd), 7.81 (6H, t), 7.90 (2H, d)
[0109] Example 9 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis〔4"-phenylnaphthalen-1"-yl〕-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 68.22 g (275 mmol) of 4-phenylnaphthalen-1-ylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 73.4 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4"-phenylnaphthalen-1"-yl]-9H-fluorene. Yield 71%, HPLC purity 99.8%, mp 230.3°C. 1 H-NMR (CDCl 3) δ1.36-1.61 (12H, m), 2.50 (4H, t), 2.97 (2H, q), 3.30 (2H, dt), 3.38 (2H, q), 3.57 (2H, dt), 4.27 (2H, s), 7.45-7.58 (20H, m), 7.66 (2H, s), 7.89 (2H, d), 7.98-8.00 (2H, m), 8.05-8.10 (2H, m)
[0110] The procedure described in step (iv) of Example 2 was followed except that 70.00 g (84.6 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[4"-phenylnaphthalen-1"-yl]-9H-fluorene, 570 ml of methyl cellosolve, 24 ml of distilled water and 7.0 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 47.95 g of the target product. Yield: 86%, HPLC purity: 99.0%, MP: 271.4°C. 1 H-NMR (DMSO-d 6 ) δ2.34 (4H, t), 2.95 (4H, dt), 4.24 (2H, t), 7.51-7.63 (20H, m), 7.72 (2H, s), 7.90-7.93 (2H, m), 7.99-8.01 (2H, m), 8.08 (2H, d)
[0111] Example 10 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-bis〔9",9”-dimethyl-9”H-fluoren-2”-yl〕-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 65.47 g (275 mmol) of 9,9-dimethyl-9H-fluoren-2-ylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2, to obtain 76.67 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[9",9"-dimethyl-9"H-fluoren-2"-yl]-9H-fluorene. Yield: 76%, HPLC purity: 91.0%, viscous solid. 1 H-NMR (CDCl 3 ) δ1.25-1.50 (12H, m), 1.58 (12H, s), 2.56 (4H, t), 2.87 (2H, q), 3.23-3.32 (4H, m), 3.51-3.57 (2H, m), 4.16 (2H, t), 7.32-7.39 (4H, m), 7.47 (2H, dd), 7.62-7.67 (4H, m), 7.69-7.72 (4H, m), 7.76-7.82 (6H, m)
[0112] The procedure described in step (iv) of Example 2 was followed except that 70.00 g (89.7 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-bis[9",9"-dimethyl-9"H-fluoren-2"-yl]-9H-fluorene, 590 ml of methyl cellosolve, 24 ml of distilled water and 6.8 ml of concentrated hydrochloric acid were used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene, 600 ml of methyl cellosolve, 25 ml of distilled water and 7 ml of concentrated hydrochloric acid, to obtain 48.21 g of the target product. Yield: 87%, HPLC purity: 96.9%, MP: 272.3°C. 1 H-NMR (DMSO-d 6) δ1.55 (12H, s), 2.42 (4H, t), 2.79 (4H, m), 4.18 (2H, t), 7.33-7.40 (4H, m), 7.59 (2H, dd), 7.76-7.79 (4H, m), 7.88 (2H, d), 7.95 (8H, dd)
[0113] Example 11 Synthesis of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-1"yl-9H-fluorene The procedure described in step (iii) of Example 2 was followed except that 47.29 g (275 mmol) of 1-naphthalenylboronic acid was used instead of 47.29 g (275 mmol) of 2-naphthaleneboronic acid in step (iii) of Example 2 to obtain 65.80 g of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthyl-1"-yl-9H-fluorene. Yield: 78%, HPLC purity: 91.0%, viscous solid. 1 H-NMR (CDCl 3 ) δ1.14-1.46(m, 12H), 2.47(t, 4H), 2.9-3.6(m, 8H), 4.2(s, 2H), 7.5-8.1(m, 20H)
[0114] The procedure described in step (iv) of Example 2 was followed except that 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-1"yl-9H-fluorene was used instead of 60.00 g (88.9 mmol) of 9,9-bis[2-(2'-tetrahydropyranyloxy)ethyl]-2,7-dinaphthalen-2"-yl-9H-fluorene in step (iv) of Example 2, to obtain 35.13 g of the target product. Yield: 78%, HPLC purity: 95.4%, viscous solid. 1 H-NMR (DMSO-d 6 ) δ2.3 (t, 4H), 2.9 (t, 4H), 4.2 (2,2H), 7.5-8.2(m, 20H)
[0115] (Comparative Synthesis Example 1) The procedure of Example 1 was repeated except that 13.41 g (0.11 mol) of phenylboronic acid was used instead of 19.17 g (0.11 mol) of naphthalene-2-boronic acid, and 19.9 g of 9,9-bis(2'-hydroxyethyl)-2,7-didiphenyl-9H-fluorene was obtained as colorless crystals.
[0116] 2. Polycarbonate resin production Example 12 20.26 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene obtained in Example 1, 8.56 g (40 mmol) of diphenyl carbonate (hereinafter sometimes abbreviated as "DPC"), and 15 μL (3 × 10 -6 (mol) was charged into a reactor equipped with a distillation device and reacted at 240°C and 100 kPa for 1 hour. After that, the degree of vacuum was adjusted to 19 kPa and the reaction was continued for 20 minutes, and then the reaction was continued at the same temperature and pressure for 70 minutes. Next, the degree of vacuum was adjusted to 16 kPa and the reaction was continued for 20 minutes, and then the degree of vacuum was adjusted to 13 kPa and the reaction was continued for 20 minutes, and then the degree of vacuum was increased to 130 Pa over 40 minutes, and the reaction was continued for 30 minutes at the same pressure until a predetermined torque was reached. The vacuum was released with nitrogen gas, and the polycarbonate resin was extracted. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 32,300, and the Tg was 135°C. The refractive index (n633) of this polycarbonate resin was 1.7608.
[0117] Comparative Example 2 In Example 12, the procedure of Example 12 was repeated except that 16.26 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene was used instead of 20.26 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-diphenyl-9H-fluorene obtained in Example 1, and a polycarbonate resin was obtained. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 28,300, and the Tg was 112°C. The refractive index (n633) of this polycarbonate resin was 1.6959.
[0118] (Example 13) 20.26 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"-yl-9H-fluorene obtained in Example 2, 8.56 g (40 mmol) of diphenyl carbonate, and 15 μL (3 × 10 -6 (mol) was charged into a reactor equipped with a distillation device and reacted at 260°C and 100 kPa for 20 minutes and at 270°C and 100 kPa for 30 minutes. After that, the degree of vacuum was adjusted to 22 kPa and the reaction was carried out for 20 minutes, and then the reaction was carried out for 60 minutes at the same temperature and pressure. Next, the degree of vacuum was adjusted to 16 kPa and the reaction was carried out for 20 minutes, and the degree of vacuum was further adjusted to 13 kPa and the reaction was carried out for 20 minutes, and then the degree of vacuum was reduced to 130 Pa over 40 minutes, and the reaction was carried out for 30 minutes at the same pressure, and when a predetermined torque was reached, the vacuum was released with nitrogen gas and the polycarbonate resin was extracted. The resulting polycarbonate resin was a crystalline polymer having a weight average molecular weight (Mw) of 4250, Tg of 115° C., and Tm of 172° C. (calorific value: 1.87 J / g). The refractive index (n633) of this polycarbonate resin was 1.7708.
[0119] Example 14 23.46 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 3, 8.56 g (40 mmol) of DPC, and 15 μL (3×10 -6The mixture was charged in a reactor equipped with a distillation device and reacted at 240°C and 100 kPa for 1 hour. The pressure was then adjusted to 22 kPa and the reaction was continued for 20 minutes, then the pressure was further adjusted to 13 kPa and the reaction was continued for 20 minutes, after which the pressure was reduced to 130 Pa over 40 minutes and the reaction was continued for 30 minutes at the same pressure. When the predetermined torque was reached, the vacuum was released with nitrogen gas and the polycarbonate resin was extracted. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 8430, and the Tg was 118°C. The refractive index (n633) of this polycarbonate resin was 1.730.
[0120] Example 15 A polycarbonate resin was produced according to the procedure described in Example 14, except that 26.35 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[3-(naphthalen-2-yl)phenyl]-9H-fluorene obtained in Example 5 was used instead of 23.46 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 3. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 5240, and the Tg was 105°C. The refractive index (n633) of this polycarbonate resin was 1.735.
[0121] Example 16 A polycarbonate resin was produced according to the procedure described in Example 14, except that 24.27 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 6 was used instead of 23.46 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 3. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 5,550, and the Tg was 126°C. The refractive index (n633) of this polycarbonate resin was 1.718.
[0122] (Example 17) A polycarbonate resin was produced according to the procedure described in Example 14, except that 23.63 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis(4"-phenoxyphenyl)-9H-fluorene obtained in Example 8 was used instead of 23.46 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 3. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 4,870, and the Tg was 67°C. The refractive index (n633) of this polycarbonate resin was 1.715.
[0123] (Example 18) A polycarbonate resin was produced according to the procedure described in Example 14, except that 26.35 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis(4"-phenylnaphthalen-1"-yl)-9H-fluorene obtained in Example 9 was used instead of 23.46 g (40 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[dibenzo[b,d]furan-4"-yl]-9H-fluorene obtained in Example 3. The resulting polycarbonate resin was a crystalline polymer having a weight average molecular weight (Mw) of 6170, a Tg of 122° C., and a Tm of 273° C. (calorific value: 8.82 J / g). The refractive index (n633) of this polycarbonate resin was 1.796.
[0124] (Example 19) 4.04 g (8 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalen-2"yl-9H-fluorene obtained in Example 2, 10.52 g (24 mmol) of 9,9-bis[4'-(2"-hydroxyethoxy)phenyl]-9H-fluorene, 1.32 g (8 mmol) of bisphenol A, 8.57 g (40 mmol) of DPC, and 15 μL (3×10 -6 The mixture was charged in a reactor equipped with a distillation device and reacted at 240°C and 100 kPa for 1 hour. The pressure was then adjusted to 22 kPa and the reaction was continued for 20 minutes, then the pressure was further adjusted to 13 kPa and the reaction was continued for 20 minutes, after which the pressure was reduced to 130 Pa over 40 minutes and the reaction was continued for 30 minutes at the same pressure. When the predetermined torque was reached, the vacuum was released with nitrogen gas and the polycarbonate resin was extracted. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 32,500, and the Tg was 139°C. The refractive index (n633) of this polycarbonate resin was 1.713. Moreover, the total light transmittance of a 500 μm thick sheet of polycarbonate resin hot-pressed at 250° C. was 82%.
[0125] (Example 20) 4.00 g (6 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-bis[4-(naphthalen-2-yl)phenyl]-9H-fluorene obtained in Example 4, 7.98 g (18 mmol) of 9,9-bis[4'-(2"-hydroxyethoxy)phenyl]-9H-fluorene, 1.39 g (6 mmol) of bisphenol A, 6.55 g (30 mmol) of DPC, and 10 μL (2 × 10 -6 mol) was charged into a reactor equipped with a distillation device and reacted at 270°C and 100 kPa for 1 hour. Thereafter, the reduced pressure was adjusted to 22 kPa and the reaction was carried out for 20 minutes, and then the reduced pressure was adjusted to 13 kPa and the reaction was carried out for 20 minutes. After that, the reduced pressure was increased to 130 Pa over 40 minutes, and the reaction was carried out for 70 minutes at the same pressure. When the predetermined torque was reached, the vacuum was released with nitrogen gas, and the polycarbonate resin was extracted. The weight average molecular weight (Mw) of the obtained polycarbonate resin was 27,800, and the Tg was 157° C. The appearance of the polycarbonate resin was colorless and transparent.
[0126] Example 21 A mixture consisting of 3.0375 g (6 mmol) of 9,9-bis(2'-hydroxyethyl)-2,7-dinaphthalene-2"yl-9H-fluorene obtained in Example 2, 6.1380 g (14 mmol) of 9,9-bis[4'-(2"-hydroxyethoxy)phenyl]-9H-fluorene, 4.8850 g (8 mmol) of 2,6-naphthalenedicarboxylic acid dimethyl ester, and 3.7 μl of titanium tetraisopropoxide (50 ppm as Ti) was charged into a reactor equipped with a distillation device and reacted at 280°C and 100 kPa for 1 hour. Thereafter, the degree of vacuum was adjusted to 20 kPa and the reaction was carried out for 20 minutes, and the degree of vacuum was further adjusted to 13 kPa and the reaction was carried out for 20 minutes. After that, the degree of vacuum was reduced to 130 Pa over 30 minutes and the reaction was carried out for 30 minutes at the same pressure. When a predetermined torque was reached, the vacuum was released with nitrogen gas and the polyester resin was extracted. The weight average molecular weight (Mw) of the obtained polyester resin was 6,300, and Tg was 118°C.
[0127] From the above, it can be understood that the polycarbonate resin obtained from the compound represented by general formula (1) according to this embodiment has a high refractive index.
[0128] This application claims priority based on Japanese Patent Application No. 2020-127221, filed on July 28, 2020, the disclosure of which is incorporated herein in its entirety.
Claims
1. A resin obtained by polymerizing a compound represented by general formula (1): 【Chemistry 1】 In the general formula (1), R 1 and R 2 represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; o and p represent an integer of 1 to 4; Ar 1 and Ar 2 each independently represent a group selected from the following: 【Chemistry 2】 In the above group, A 1 to A 5 and B 1 to B 5 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group, at least one of A 1 to A 5 is a -Y 1 -Ar 3 group, at least one of B 1 to B 5 is a -Y 2 -Ar 4 group, Y 1 and Y 2 each represent a single bond or a linking group, and Ar 3 and Ar 4 each represent an aromatic group; X 1 and X 2 are —O—, —S—, —NR′— or —C(Me) 2 —; Z 1 to Z 4 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; R 3 to R 6 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group.
2. The resin described in claim 1, wherein o and p in the general formula (1) are 2.
3. A polycarbonate resin derived from a compound represented by general formula (1). 【Chemistry 3】 In the general formula (1), R 1 and R 2 represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; o and p represent an integer of 1 to 4; Ar 1 and Ar 2 each independently represent a group selected from the following: 【Chemistry 4】 In the above group, A 1 to A 5 and B 1 to B 5 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group, at least one of A 1 to A 5 is a -Y 1 -Ar 3 group, at least one of B 1 to B 5 is a -Y 2 -Ar 4 group, Y 1 and Y 2 each represent a single bond or a linking group, and Ar 3 and Ar 4 each represent an aromatic group; X 1 and X 2 are —O—, —S—, —NR′— or —C(Me) 2 —; Z 1 to Z 4 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group; R 3 to R 6 each represent a hydrogen atom, a hydrocarbon group, or a heteroatom-containing hydrocarbon group.
4. The resin described in claim 2, wherein o and p in the general formula (1) are 2.
5. An optically molded article comprising the resin according to claim 1 or 2.
6. An optical molded article comprising the polycarbonate resin according to claim 3 or 4.
7. 6. The optical molded article according to claim 5, which is an optical lens.
8. The optical molded article according to claim 5, which is an optical film.
Citation Information
Patent Citations
Alcohol-soluble hole-transporting molecular material and preparation method thereof
CN102649766A
Fluorene-based resin composition and its shaped article
JP2005187661A
Optical lens
JP2005241962A
Polycarbonate resin and optical film
JP2008222965A
Electrophotographic photoreceptor, electrophotographic apparatus, process cartridge, and condensed polycyclic aromatic compound
JP2014197173A