Composition, resist underlayer film, method for forming resist underlayer film, method for producing patterned substrate, and compound

A composition with an aromatic hydrocarbon ring structure and solvent improves etching resistance and embeddability of resist underlayer films, addressing the limitations of existing films in semiconductor manufacturing for complex trench patterns.

JP7589693B2Active Publication Date: 2024-11-26JSR CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021546921
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-17
Filing Date
2020-09-15
Publication Date
2024-11-26
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Existing resist underlayer films in semiconductor manufacturing lack sufficient etching resistance, heat resistance, and embeddability, especially when forming patterns with varying trench aspect ratios.

Method used

A composition containing a compound with an aromatic hydrocarbon ring structure and a partial structure, along with a solvent, is used to form a resist underlayer film that enhances etching resistance, heat resistance, and embeddability.

Benefits of technology

The composition forms a film with excellent etching resistance, heat resistance, and embeddability, enabling the production of patterned substrates with improved patterning quality for future miniaturized semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589693000001
    Figure 0007589693000001
  • Figure 0007589693000002
    Figure 0007589693000002
  • Figure 0007589693000003
    Figure 0007589693000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a composition capable of forming a film that exhibits excellent etching resistance, heat resistance and embedding properties; a resist underlayer film; a method for forming a resist underlayer film; a method for producing a patterned substrate; and a compound. The present invention is a composition which contains a solvent and a compound having an aromatic hydrocarbon ring structure and a partial structure represented by formula (1). The number of carbon atoms in the aromatic hydrocarbon ring structure is 25 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a composition, a resist underlayer film, a method for forming a resist underlayer film, a method for producing a patterned substrate, and a compound. [Background technology]

[0002] In the manufacture of semiconductor devices, for example, a multilayer resist process is used in which a resist pattern is formed by exposing and developing a resist film laminated on a substrate via a resist underlayer film such as an organic underlayer film or a silicon-containing film. In this process, the resist underlayer film is etched using the resist pattern as a mask, and the substrate is further etched using the resulting resist underlayer film pattern as a mask, thereby forming a desired pattern on the substrate and obtaining a patterned substrate (see JP 2004-177668 A).

[0003] Various studies have been conducted on materials used in such compositions for forming resist underlayer films (see International Publication No. 2011 / 108365). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2004-177668 [Patent Document 2] International Publication No. 2011 / 108365 Summary of the Invention [Problem to be solved by the invention]

[0005] In a multilayer resist process, the organic underlayer film serving as the resist underlayer film is required to have etching resistance and heat resistance.

[0006] Recently, there has been an increase in the number of cases where patterns are formed on substrates having multiple types of trenches, particularly trenches having different aspect ratios, and in such cases, the composition for forming the resist underlayer film is required to be able to sufficiently fill these trenches, i.e., to have excellent filling properties.

[0007] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a composition, a resist underlayer film, a method for forming a resist underlayer film, a method for producing a patterned substrate, and a compound that are capable of forming a film that is excellent in etching resistance, heat resistance, and embedding ability. [Means for solving the problem]

[0008] The invention made to solve the above problem is a composition containing a compound (hereinafter also referred to as "compound [A1]") having an aromatic hydrocarbon ring structure and a partial structure represented by the following formula (1), and a solvent (hereinafter also referred to as "solvent [B]"), wherein the aromatic hydrocarbon ring structure has 25 or more carbon atoms. [ka] (In formula (1), X is a group represented by the following formula (i), (ii), (iii), or (iv). * represents a bonding site to two adjacent carbon atoms constituting the aromatic hydrocarbon ring structure.) [ka] (In formula (i), R 1 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 2 is a monovalent organic group having 1 to 20 carbon atoms. In formula (ii), R 3 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 4 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iii), R 5 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iv), R 6is a monovalent organic group having 1 to 20 carbon atoms.

[0009] Another invention made to solve the above problems is a resist underlayer film formed from the composition.

[0010] Yet another invention made to solve the above-mentioned problems is a method for forming a resist underlayer film, comprising a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate, wherein the composition for forming a resist underlayer film is the composition.

[0011] Another invention made to solve the above-mentioned problems is a method for producing a patterned substrate, comprising the steps of: applying a composition for forming a resist underlayer film directly or indirectly to a substrate; forming a resist pattern directly or indirectly on the resist underlayer film formed by the application step; and performing etching using the resist pattern as a mask, wherein the composition for forming a resist underlayer film is the composition.

[0012] Another invention made to solve the above problems provides a compound having an aromatic hydrocarbon ring structure and a partial structure represented by the following formula (2): The compound has an aromatic hydrocarbon ring structure with 25 or more carbon atoms (hereinafter, also referred to as "compound [A2]"). [ka] (In formula (2), Y is a group represented by the following formula (v), (vi), (vii), or (viii). * represents a bonding site to two adjacent carbon atoms constituting the aromatic hydrocarbon ring structure.) [ka] (In formula (v), R 7 and R 8 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (vi), R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (vii), R 11 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (viii), R 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. [Effects of the Invention]

[0013] The composition of the present invention can form a film having excellent etching resistance, heat resistance, and embedding ability. The resist underlayer film of the present invention has excellent etching resistance, heat resistance, and embedding ability. The method for forming a resist underlayer film of the present invention can form a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability. The method for producing a patterned substrate of the present invention can form a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability, thereby obtaining a well-patterned substrate. The compound of the present invention can be suitably used as a component of a composition for forming a resist underlayer film. Therefore, these compounds can be suitably used in the production of semiconductor devices, which are expected to become even more miniaturized in the future. DETAILED DESCRIPTION OF THE INVENTION

[0014] The composition, resist underlayer film, method for forming a resist underlayer film, method for producing a patterned substrate, and compound of the present invention will be described in detail below.

[0015] <Composition> The composition contains the compound [A1] and the solvent [B]. The composition may contain any optional components as long as the optional components do not impair the effects of the present invention.

[0016] The composition contains the compound [A1] and the solvent [B], and thus can form a film having excellent etching resistance, heat resistance, and embedding ability. Therefore, the composition can be used as a composition for forming a film. More specifically, the composition can be suitably used as a composition for forming a resist underlayer film in a multilayer resist process.

[0017] Each component contained in the composition will be described below.

[0018] <[A1] Compound> The compound [A1] is a compound having an aromatic hydrocarbon ring structure (hereinafter also referred to as "aromatic hydrocarbon ring structure (I)") and a partial structure represented by the following formula (1) (hereinafter also referred to as "partial structure (II)"), which will be described later.

[0019] [Aromatic hydrocarbon ring structure (I)] The aromatic hydrocarbon ring structure (I) is an aromatic hydrocarbon ring structure having 25 or more carbon atoms. In this specification, the "number of carbon atoms in the aromatic hydrocarbon ring structure (I)" means the number of carbon atoms constituting the ring structure of the aromatic hydrocarbon ring structure (I). The "number of carbon atoms in the aromatic hydrocarbon ring structure (I)" does not include the number of carbon atoms constituting the partial structure (II).

[0020] The lower limit of the number of carbon atoms in the aromatic hydrocarbon ring structure (I) is 25, preferably 35, and more preferably 40. The upper limit of the number of carbon atoms is not particularly limited and is, for example, 100. When the number of carbon atoms in the aromatic hydrocarbon ring structure (I) is 25 or more, a film having excellent etching resistance and heat resistance can be formed.

[0021] Examples of the aromatic hydrocarbon ring structure (I) include a structure containing a fused polycyclic structure, a structure containing a ring assembly structure, or a combination thereof. In this specification, the term "fused polycyclic structure" refers to a ring structure among polycyclic structures having two or more aromatic hydrocarbon rings, in which one aromatic hydrocarbon ring and another aromatic hydrocarbon ring are bonded together by sharing two carbon atoms. The term "ring assembly structure" refers to a ring structure among polycyclic structures having two or more aromatic hydrocarbon rings, in which one aromatic hydrocarbon ring and another aromatic hydrocarbon ring are bonded together via a single bond, rather than by sharing a carbon atom.

[0022] The fused polycyclic structure is not particularly limited as long as it has 25 or more carbon atoms, and examples thereof include a trinaphthylene structure (30 carbon atoms), a heptaphene structure (30 carbon atoms), a heptacene structure (30 carbon atoms), a pyranthrene structure (30 carbon atoms), an ovalene structure (32 carbon atoms), and a hexabenzocoronene structure (42 carbon atoms). As the fused polycyclic structure, a hexabenzocoronene structure is preferred.

[0023] Fused polycyclic structures are generally classified into four types based on the suffix of the name of the fused polycyclic structure: linear fused ring systems with the suffix -acene; winged fused ring systems with the suffix -aphene; fused ring systems with two identical rings arranged side by side with the suffix -alene; and fused ring systems with benzene rings centered around a single ring with the suffix -phenylene. In this classification, fused ring systems with benzene rings centered around a single ring with the suffix -phenylene are preferred. Fused polycyclic structures with benzene rings centered around a single ring with the suffix -phenylene have a higher carbon atom content than other fused polycyclic structures, even when the number of carbon atoms is the same, thereby improving the etching resistance of films formed from the composition. The hexabenzocoronene structure described above is included in the fused ring systems with benzene rings centered around a single ring with the suffix -phenylene.

[0024] The ring assembly structure is not particularly limited as long as it has 25 or more carbon atoms, and examples thereof include a tetraphenylbenzene structure (carbon number: 30), a pentaphenylbenzene structure (carbon number: 36), a hexaphenylbenzene structure (carbon number: 42), etc. As the ring assembly structure, a hexaphenylbenzene structure is preferred.

[0025] The structure combining a fused polycyclic structure and a ring assembly structure is not particularly limited as long as it has 25 or more carbon atoms, and examples thereof include a diphenylpyrene structure (28 carbon atoms), a dinaphthylpyrene structure (36 carbon atoms), and a tetraphenylpyrene structure (40 carbon atoms).

[0026] The aromatic hydrocarbon ring structure (I) is preferably a structure containing a fused polycyclic structure. When the aromatic hydrocarbon ring structure (I) is a structure containing a fused polycyclic structure, the etching resistance and heat resistance of the film formed from the composition can be further improved.

[0027] [Substructure (II)] The partial structure (II) is a partial structure represented by the following formula (1).

[0028] [ka]

[0029] In the above formula (1), X is a group represented by the following formula (i), (ii), (iii), or (iv) (hereinafter also referred to as "group (X)"), which will be described later. * each represents a bonding site to two adjacent carbon atoms constituting the above aromatic hydrocarbon ring structure (aromatic hydrocarbon ring structure (I)).

[0030] In the compound [A1], the partial structure (II) is bonded to the aromatic hydrocarbon ring structure (I). More specifically, the partial structure (II) is bonded to two adjacent carbon atoms constituting the aromatic hydrocarbon ring structure (I).

[0031] The lower limit of the number of partial structures (II) in the compound [A1] is 1, and preferably 2. The upper limit of the number of the partial structures (II) is not particularly limited, and is preferably 10, and more preferably 6. When the compound [A1] has two or more partial structures (II), X in the formula (1) above may be the same or different.

[0032] (Group(X)) The group (X) is a group represented by the following formula (i), (ii), (iii) or (iv) (hereinafter also referred to as "groups (Xi) to (X-iv)").

[0033] [ka]

[0034] In the above formula (i), R 1 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 2 is a monovalent organic group having 1 to 20 carbon atoms.

[0035] In the above formula (ii), R 3 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 4 is a monovalent organic group having 1 to 20 carbon atoms.

[0036] In the above formula (iii), R 5 is a monovalent organic group having 1 to 20 carbon atoms.

[0037] In the above formula (iv), R 6 is a monovalent organic group having 1 to 20 carbon atoms.

[0038] As used herein, "organic group" means a group containing at least one carbon atom.

[0039] R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Examples of the monovalent organic group having 1 to 20 carbon atoms and represented by the formula (I) include a monovalent hydrocarbon group having 1 to 20 carbon atoms, a group having a divalent heteroatom-containing group between carbon atoms of this hydrocarbon group (hereinafter also referred to as "group (α)"), a group in which some or all of the hydrogen atoms of the hydrocarbon group have been substituted with monovalent heteroatom-containing groups (hereinafter also referred to as "group (β)"), and a group in which some or all of the hydrogen atoms of the group (α) have been substituted with monovalent heteroatom-containing groups (hereinafter also referred to as "group (γ)").

[0040] In this specification, the term "hydrocarbon group" includes linear hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. This "hydrocarbon group" includes saturated hydrocarbon groups and unsaturated hydrocarbon groups. The term "linear hydrocarbon group" refers to a hydrocarbon group that does not contain a ring structure and is composed only of a linear structure, and includes both linear hydrocarbon groups and branched hydrocarbon groups. The term "alicyclic hydrocarbon group" refers to a hydrocarbon group that contains only an alicyclic structure as a ring structure and does not contain an aromatic ring structure, and includes both monocyclic alicyclic hydrocarbon groups and polycyclic alicyclic hydrocarbon groups (however, it does not have to be composed only of an alicyclic structure and may contain a linear structure as part of it). The term "aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as a ring structure (however, it does not have to be composed only of an aromatic ring structure and may contain an alicyclic structure or a linear structure as part of it).

[0041] Examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and groups formed by combining these groups.

[0042] Examples of the monovalent chain hydrocarbon group having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, sec-butyl, and tert-butyl; alkenyl groups such as ethenyl, propenyl, and butenyl; and alkynyl groups such as ethynyl, propynyl, and butynyl.

[0043] Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include cycloalkyl groups such as a cyclopentyl group and a cyclohexyl group; cycloalkenyl groups such as a cyclopropenyl group, a cyclopentenyl group and a cyclohexenyl group; bridged ring saturated hydrocarbon groups such as a norbornyl group, an adamantyl group and a tricyclodecyl group; and bridged ring unsaturated hydrocarbon groups such as a norbornenyl group and a tricyclodecenyl group.

[0044] Examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a naphthyl group, an anthracenyl group, and a pyrenyl group.

[0045] Examples of heteroatoms constituting the divalent or monovalent heteroatom-containing group include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, silicon atoms, and halogen atoms. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.

[0046] Examples of the divalent heteroatom-containing group include -CO-, -CS-, -NH-, -O-, -S-, and combinations of these groups.

[0047] Examples of the monovalent heteroatom-containing group include a hydroxy group, a sulfanyl group, a cyano group, a nitro group, and a halogen atom.

[0048] R 1 , R 2 , R 3 , R 4 , R 5 and R 6 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (I) is preferably a group (hereinafter also referred to as "group (x)") that has the property of being eliminated from the compound [A1] by heating and the property of increasing the solubility of the compound [A1] in the solvent [B]. When the group (x) has the property of being eliminated from the compound [A1], the carbon atom content of the film formed from the composition is increased, and as a result, etching resistance can be further improved. Furthermore, when the group (x) has the property of increasing the solubility of the compound [A1] in the solvent [B], the coatability of the composition can be improved. Note that heating conditions under which the group (x) is eliminated from the compound [A1] include, for example, conditions similar to the heating conditions in the heating step included in the method for forming the resist underlayer film described below.

[0049] Examples of the group (x) include groups represented by the following formulae (x-1) to (x-12) (hereinafter also referred to as "groups (x-1) to (x-12)").

[0050] [ka]

[0051] In the above formulas (x-1) to (x-12), ** represents the bonding site to the carbon atom or nitrogen atom in the above formula (i), (ii), (iii) or (iv).

[0052] The group (x) is preferably the group (x-1), the group (x-3), the group (x-8) or the group (x-9).

[0053] The group (X) is preferably the group (Xi) or the group (X-ii).

[0054] Examples of the compound [A1] include compounds represented by the following formulas (A1-1) to (A1-8) (hereinafter also referred to as "compounds (A1-1) to (A1-8)").

[0055] [ka]

[0056] [ka]

[0057] In the above formulas (A1-1) to (A1-8), X has the same meaning as in the above formula (1).

[0058] The compound [A1] is preferably the compound (A1-1), the compound (A1-2), the compound (A1-3) or the compound (A1-5), and more preferably the compound (A1-1), the compound (A1-2) or the compound (A1-3).

[0059] The compound [A1] may have a substituent other than the aromatic hydrocarbon ring structure (I) and partial structure (II) described above, or may not have the above substituent. The compound [A1] is preferably one that does not have the above substituent. When the compound [A1] does not have a substituent, the carbon atom content of the compound [A1] is higher than when the compound [A1] has a substituent, and therefore the etching resistance of the film formed from the composition can be further improved.

[0060] Examples of the substituent include a halogen atom, a hydroxy group, a nitro group, and a monovalent organic group having 1 to 20 carbon atoms. Examples of the monovalent organic group having 1 to 20 carbon atoms as the substituent include R 1 ~R 6 Examples of the monovalent organic group having 1 to 20 carbon atoms and represented by the following formula include the same groups as those exemplified above.

[0061] When the compound [A1] has a substituent, the position at which the substituent is bonded is not particularly limited, and the substituent may be bonded to the aromatic hydrocarbon ring structure (I) or the partial structure (II).

[0062] The lower limit of the molecular weight of the compound [A1] is preferably 600, more preferably 700, even more preferably 800, and particularly preferably 900. The upper limit of the molecular weight is preferably 5,000, more preferably 4,000, even more preferably 3,500, and particularly preferably 3,000.

[0063] The lower limit of the content of the compound [A] in the composition is preferably 60 mass %, more preferably 70 mass %, further preferably 80 mass %, and particularly preferably 90 mass %, based on all components in the composition other than the solvent [B]. The upper limit of the content is, for example, 100 mass %.

[0064] [[A1] Compound synthesis method] The compound [A1] can be synthesized by a conventional method, for example, according to the following synthesis scheme.

[0065] [ka]

[0066] In reaction 1, bis(2-fluorenyl)acetylenes are reacted with each other to synthesize the compound represented by the above formula (a-3), which is an intermediate.

[0067] In reaction 2, the compound represented by formula (a-3) synthesized in reaction 1 is cyclized in the presence of a catalyst or the like to synthesize a compound represented by formula (a-4). In reaction 3, the compound represented by formula (a-4) synthesized in reaction 2 is reacted with t-butyl acrylate, which provides the group (x), to synthesize a compound represented by formula (A-3). The compound represented by formula (A-3) is an example of compound (A1-2).

[0068] In reaction 4, the compound represented by formula (a-3) synthesized in reaction 1 is reacted with propargyl bromide as a compound that provides the group (x) to synthesize a compound represented by formula (A-5). The compound represented by formula (A-5) is an example of the compound (A1-5).

[0069] <[B] Solvent> The solvent [B] is not particularly limited as long as it can dissolve or disperse the compound [A1] and any optional components contained as needed.

[0070] Examples of the solvent [B] include hydrocarbon solvents, ester solvents, alcohol solvents, ketone solvents, ether solvents, nitrogen-containing solvents, etc. The solvent [B] can be used alone or in combination of two or more.

[0071] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as n-pentane, n-hexane, and cyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene.

[0072] Examples of ester-based solvents include carbonate-based solvents such as diethyl carbonate, acetate monoester-based solvents such as methyl acetate and ethyl acetate, lactone-based solvents such as γ-butyrolactone, polyhydric alcohol partial ether carboxylate-based solvents such as diethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate, and lactate-based solvents such as methyl lactate and ethyl lactate.

[0073] Examples of alcohol solvents include monoalcohol solvents such as methanol, ethanol, and n-propanol, and polyalcohol solvents such as ethylene glycol and 1,2-propylene glycol.

[0074] Examples of the ketone solvent include chain ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, and cyclic ketone solvents such as cyclohexanone.

[0075] Examples of ether solvents include chain ether solvents such as n-butyl ether, polyhydric alcohol ether solvents such as cyclic ether solvents such as tetrahydrofuran, and polyhydric alcohol partial ether solvents such as diethylene glycol monomethyl ether.

[0076] Examples of the nitrogen-containing solvent include chain nitrogen-containing solvents such as N,N-dimethylacetamide, and cyclic nitrogen-containing solvents such as N-methylpyrrolidone.

[0077] The solvent (B) is preferably an ester solvent or a ketone solvent, more preferably a polyhydric alcohol partial ether carboxylate solvent or a cyclic ketone solvent, and even more preferably propylene glycol monomethyl ether acetate or cyclohexanone.

[0078] The lower limit of the content of the solvent [B] in the composition is preferably 50% by mass, more preferably 60% by mass, and even more preferably 70% by mass, and the upper limit of the content is preferably 99.9% by mass, more preferably 99% by mass, and even more preferably 95% by mass.

[0079] [Optional ingredients] The composition may contain optional components within the range that does not impair the effects of the present invention. Examples of optional components include an acid generator, a crosslinking agent, a surfactant, etc. The optional components may be used alone or in combination of two or more. The content ratio of the optional components in the composition may be appropriately determined depending on the type of optional component, etc.

[0080] [Method for preparing the composition] The composition can be prepared by mixing the compound [A1], the solvent [B], and, if necessary, any optional components in a predetermined ratio, and then filtering the resulting mixture preferably through a membrane filter or the like having a pore size of 0.1 μm or less.

[0081] <Resist Underlayer Film> The resist underlayer film is formed from the composition described above and has excellent etching resistance, heat resistance, and embedding ability.

[0082] <Method for forming resist underlayer film> The method for forming a resist underlayer film includes a step of directly or indirectly applying a composition for forming a resist underlayer film to a substrate (hereinafter also referred to as a "coating step").

[0083] In the method for forming a resist underlayer film, the composition described above is used as a composition for forming a resist underlayer film in the coating step, so that a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability can be formed.

[0084] The method for forming a resist underlayer film preferably further comprises a step of heating the coating film formed in the coating step (hereinafter also referred to as a "heating step").

[0085] Each step of the method for forming a resist underlayer film will be described below.

[0086] [Coating process] In this step, the composition for forming a resist underlayer film is applied directly or indirectly to a substrate. In this step, the composition for forming a resist underlayer film is the composition described above.

[0087] The method for applying the composition for forming a resist underlayer film is not particularly limited, and can be any appropriate method such as spin coating, casting coating, roll coating, etc. This forms a coating film, and the resist underlayer film is formed by volatilization of the solvent [B].

[0088] Examples of the substrate include metal or semimetal substrates such as silicon substrates, aluminum substrates, nickel substrates, chromium substrates, molybdenum substrates, tungsten substrates, copper substrates, tantalum substrates, and titanium substrates, among which silicon substrates are preferred.The substrate may also be a substrate on which a silicon nitride film, an alumina film, a silicon dioxide film, a tantalum nitride film, a titanium nitride film, or the like is formed.

[0089] An example of the case where the composition for forming a resist underlayer film is indirectly applied to a substrate is the case where the composition for forming a resist underlayer film is applied onto a silicon-containing film, which will be described later, formed on the substrate.

[0090] [Heating process] In this step, the coating film formed in the coating step is heated. Heating the coating film promotes the formation of a resist underlayer film. More specifically, heating the coating film promotes the elimination of the group (x) from the compound [A1] and the volatilization of the solvent [B].

[0091] The coating film may be heated in an air atmosphere or a nitrogen atmosphere. The lower limit of the heating temperature is preferably 150°C, more preferably 200°C. The upper limit of the heating temperature is preferably 600°C, more preferably 500°C. The lower limit of the heating time is preferably 15 seconds, more preferably 30 seconds. The upper limit of the heating time is preferably 1,200 seconds, more preferably 600 seconds.

[0092] The lower limit of the average thickness of the resist underlayer film formed is preferably 30 nm, more preferably 50 nm, and even more preferably 100 nm. The upper limit of the average thickness is preferably 3,000 nm, more preferably 2,000 nm, and even more preferably 500 nm. The average thickness of the resist underlayer film is a value measured using a spectroscopic ellipsometer (JAWOOLLAM's "M2000D").

[0093] <Method for manufacturing a patterned substrate> The method for manufacturing the patterned substrate includes a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate (hereinafter also referred to as a "coating step"), a step of forming a resist pattern directly or indirectly on the resist underlayer film formed by the coating step (hereinafter also referred to as a "resist pattern forming step"), and a step of performing etching using the resist pattern as a mask (hereinafter also referred to as an "etching step").

[0094] According to the method for producing a patterned substrate, by using the composition described above as a composition for forming a resist underlayer film in the coating step, a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability can be formed, and therefore a patterned substrate having a good pattern shape can be produced.

[0095] The method for producing a patterned substrate may further include a step of heating the coating film formed in the coating step (hereinafter also referred to as a "heating step"), if necessary.

[0096] The method for producing a patterned substrate may further include, as necessary, a step of forming a silicon-containing film directly or indirectly on the resist underlayer film formed by the coating step or the heating step (hereinafter also referred to as a "silicon-containing film forming step").

[0097] Each step of the method for manufacturing the patterned substrate will be described below.

[0098] [Coating process] In this step, the composition for forming a resist underlayer film is applied directly or indirectly to a substrate, and this step is the same as the application step in the method for forming the resist underlayer film described above.

[0099] [Heating process] In this step, the coating film formed in the coating step is heated, which is the same as the heating step in the method for forming the resist underlayer film described above.

[0100] [Silicon-containing film formation process] In this process, a silicon-containing film is formed directly or indirectly on the resist underlayer film formed by the coating process or the heating process.When the silicon-containing film is formed indirectly on the resist underlayer film, for example, a surface-modified film of the resist underlayer film is formed on the resist underlayer film.The surface-modified film of the resist underlayer film is, for example, a film whose contact angle with water is different from that of the resist underlayer film.

[0101] The silicon-containing film can be formed by coating a silicon-containing film-forming composition, chemical vapor deposition (CVD), atomic layer deposition (ALD), or the like. Examples of methods for forming a silicon-containing film by coating a silicon-containing film-forming composition include a method in which the silicon-containing film-forming composition is directly or indirectly coated onto the resist underlayer film, and the resulting coated film is then cured by exposure and / or heating. Examples of commercially available silicon-containing film-forming compositions that can be used include "NFC SOG01," "NFC SOG04," and "NFC SOG080" (all from JSR Corporation). Chemical vapor deposition (CVD) or atomic layer deposition (ALD) can form, for example, silicon oxide films, silicon nitride films, silicon oxynitride films, and amorphous silicon films.

[0102] Examples of radiation used for the exposure include electromagnetic waves such as visible light, ultraviolet light, far ultraviolet light, X-rays and gamma rays, and particle beams such as electron beams, molecular beams and ion beams.

[0103] The lower limit of the temperature when heating the coating film is preferably 90°C, more preferably 150°C, and even more preferably 200°C. The upper limit of the temperature is preferably 550°C, more preferably 450°C, and even more preferably 300°C.

[0104] The lower limit of the average thickness of the silicon-containing film is preferably 1 nm, more preferably 10 nm, and even more preferably 20 nm. The upper limit is preferably 20,000 nm, more preferably 1,000 nm, and even more preferably 100 nm. The average thickness of the silicon-containing film is a value measured using the spectroscopic ellipsometer, similar to the average thickness of the resist underlayer film.

[0105] [Resist pattern formation process] In this step, a resist pattern is formed directly or indirectly on the resist underlayer film.Methods for carrying out this step include, for example, a method using a resist composition, a method using a nanoimprint method, a method using a self-assembling composition, etc.An example of a case where a resist pattern is formed indirectly on the resist underlayer film is, for example, a case where a resist pattern is formed on the silicon-containing film.

[0106] Specifically, in the method using the resist composition, the resist composition is applied so that the resist film to be formed has a predetermined thickness, and then the applied film is pre-baked to volatilize the solvent in the applied film, thereby forming a resist film.

[0107] Examples of the resist composition include a positive or negative chemically amplified resist composition that contains a radiation-sensitive acid generator, a positive resist composition that contains an alkali-soluble resin and a quinone diazide-based photosensitizer, and a negative resist composition that contains an alkali-soluble resin and a crosslinking agent.

[0108] The lower limit of the content of all components other than the solvent in the resist composition is preferably 0.3% by mass, more preferably 1% by mass. The upper limit of the content is preferably 50% by mass, more preferably 30% by mass. The resist composition is generally filtered, for example, through a filter with a pore size of 0.2 μm or less, before being used to form a resist film. In this step, a commercially available resist composition can also be used as is.

[0109] Examples of methods for applying the resist composition include spin coating. The pre-baking temperature and time can be adjusted appropriately depending on the type of resist composition used. The lower limit of the temperature is preferably 30°C, more preferably 50°C. The upper limit of the temperature is preferably 200°C, more preferably 150°C. The lower limit of the time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the time is preferably 600 seconds, more preferably 300 seconds.

[0110] Next, the resist film formed above is exposed by selective irradiation with radiation. The radiation used for exposure can be appropriately selected depending on the type of radiation-sensitive acid generator used in the resist composition, and examples include visible light, ultraviolet light, far ultraviolet light, electromagnetic waves such as X-rays and gamma rays, and particle beams such as electron beams, molecular beams, and ion beams. Among these, far ultraviolet light is preferred, and KrF excimer laser light (wavelength 248 nm), ArF excimer laser light (wavelength 193 nm), F2 excimer laser light (wavelength 157 nm), Kr2 excimer laser light (wavelength 147 nm), ArKr excimer laser light (wavelength 134 nm), or extreme ultraviolet light (wavelength 13.5 nm, etc., hereinafter also referred to as "EUV") is more preferred, and KrF excimer laser light, ArF excimer laser light, or EUV is even more preferred.

[0111] After the exposure, post-baking can be performed to improve resolution, pattern profile, developability, etc. The temperature and time of this post-baking can be appropriately determined depending on the type of resist composition used, etc. The lower limit of the temperature is preferably 50°C, more preferably 70°C. The upper limit of the temperature is preferably 200°C, more preferably 150°C. The lower limit of the post-baking time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the time is preferably 600 seconds, more preferably 300 seconds.

[0112] Next, the exposed resist film is developed with a developer to form a resist pattern. This development may be alkaline or organic solvent development. In the case of alkaline development, examples of the developer include aqueous solutions of basic compounds such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide, pyrrole, piperidine, choline, 1,8-diazabicyclo[5.4.0]-7-undecene, and 1,5-diazabicyclo[4.3.0]-5-nonene. These aqueous solutions may also contain an appropriate amount of a water-soluble organic solvent, such as an alcohol (e.g., methanol or ethanol), a surfactant, or the like. In the case of organic solvent development, examples of the developer include the various organic solvents exemplified as solvent [B] in the composition described above.

[0113] After development with the developer, the resist is washed and dried to form a desired resist pattern.

[0114] [Etching process] In this step, etching is performed using the resist pattern as a mask. The etching may be performed once or multiple times, i.e., sequentially using the pattern obtained by etching as a mask. From the viewpoint of obtaining a pattern with a better shape, multiple times is preferred. When performing multiple etchings, for example, etching is performed sequentially in the order of the silicon-containing film, the resist underlayer film, and the substrate. Examples of etching methods include dry etching and wet etching. From the viewpoint of obtaining a better pattern shape on the substrate, dry etching is preferred. For this dry etching, a gas plasma such as oxygen plasma is used. By the above etching, a patterned substrate having a predetermined pattern is obtained.

[0115] Dry etching can be performed using, for example, a known dry etching apparatus. The etching gas used for dry etching can be appropriately selected depending on the mask pattern, the elemental composition of the film to be etched, etc., and includes, for example, fluorine-based gases such as CHF3, CF4, C2F6, C3F8, and SF6; chlorine-based gases such as Cl2 and BCl3; oxygen-based gases such as O2, O3, and H2O; reducing gases such as H2, NH3, CO, CO2, CH4, C2H2, C2H4, C2H6, C3H4, C3H6, C3H8, HF, HI, HBr, HCl, NO, NH3, and BCl3; and inert gases such as He, N2, and Ar. These gases can also be used in combination. When etching a substrate using a resist underlayer film pattern as a mask, a fluorine-based gas is usually used.

[0116] <[A2] Compound> The compound [A2] has an aromatic hydrocarbon ring structure (hereinafter also referred to as "aromatic hydrocarbon ring structure (I')") and a partial structure represented by the following formula (2) described below (hereinafter also referred to as "partial structure (II')"), and the aromatic hydrocarbon ring structure has 25 or more carbon atoms.

[0117] The compound [A2] can be suitably used as a component of the composition described above, and can also be used as an intermediate in synthesizing the compound [A1] described above.

[0118] [Aromatic hydrocarbon ring structure (I')] The aromatic hydrocarbon ring structure (I') is an aromatic hydrocarbon ring structure having a carbon number of 25 or more. The aromatic hydrocarbon ring structure (I') is the same as the aromatic hydrocarbon ring structure (I) in the compound [A1] described above.

[0119] [Substructure (II')] The partial structure (II') is a partial structure represented by the following formula (2).

[0120] [ka]

[0121] In the above formula (2), Y is a group represented by the following formula (v), (vi), (vii), or (viii) (hereinafter also referred to as "group (Y)"), which will be described later. * each represents a bonding site to two adjacent carbon atoms constituting the above aromatic hydrocarbon ring structure (aromatic hydrocarbon ring structure (I')).

[0122] In the compound [A2], the partial structure (II') is bonded to the aromatic hydrocarbon ring structure (I'). More specifically, the partial structure (II') is bonded to two adjacent carbon atoms constituting the aromatic hydrocarbon ring structure (I').

[0123] The lower limit of the number of partial structures (II') in the compound [A2] is 1, and preferably 2. The upper limit of the number of the partial structures (II') is not particularly limited, and is preferably 10, and more preferably 6. When the compound [A2] has two or more partial structures (II'), the Ys in the formula (2) above may be the same or different.

[0124] (Group(Y)) The group (Y) is a group represented by the following formula (v), (vi), (vii) or (viii) (hereinafter also referred to as "groups (Yv) to (Y-viii)").

[0125] [ka]

[0126] In the above formula (v), R 7 and R 8 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0127] In the above formula (vi), R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0128] In the above formula (vii), R 11is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0129] In the above formula (viii), R 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0130] R 7 , R 8 , R 9 , R 10 , R 11 and R 12 Examples of the monovalent organic group having 1 to 20 carbon atoms represented by the formula (i) to (iv) include R 1 ~R 6 Examples of the monovalent organic group having 1 to 20 carbon atoms and represented by the following formula include the same groups as those exemplified above.

[0131] The group (Y) is R in each of the above formulas (v) to (viii). 7 ~R 12 are all hydrogen atoms (hereinafter also referred to as "group (Y-1)"), or R 7 ~R 12 It is preferable that at least one of the groups is a monovalent organic group having 1 to 20 carbon atoms (hereinafter also referred to as "group (Y-2)").

[0132] When the compound [A2] has a group (Y-1), the compound [A2] is useful as an intermediate for the compound [A1] described above.

[0133] When the compound [A2] has a group (Y-2), this compound [A2] can be suitably used as a component of the composition, similar to the compound [A1] described above.

[0134] As the group (Y), the group (Yv) is preferred.

[0135] Examples of the compound [A2] include compounds represented by the following formulas (A2-1) to (A2-8) (hereinafter also referred to as "compounds (A2-1) to (A2-8)").

[0136] [ka]

[0137] [ka]

[0138] In the above formulas (A2-1) to (A2-8), Y has the same meaning as in the above formula (2).

[0139] The compound [A2] is preferably the compound (A2-1), the compound (A2-2), the compound (A2-3) or the compound (A2-5), more preferably the compound (A2-1), the compound (A2-2) or the compound (A2-3).

[0140] The compound [A2] may have a substituent other than the aromatic hydrocarbon ring structure (I') and the partial structure (II') described above, or may not have the above substituent. The compound [A2] is preferably one that does not have the above substituent.

[0141] Examples of the substituent include the same groups as those exemplified as the substituents that the compound [A1] may have.

[0142] When the compound [A2] has a substituent, the position at which the substituent is bonded is not particularly limited, and the substituent may be bonded to the aromatic hydrocarbon ring structure (I') or the partial structure (II').

[0143] The lower limit of the molecular weight of the compound [A2] is preferably 600, more preferably 700, even more preferably 800, and particularly preferably 900. The upper limit of the molecular weight is preferably 5,000, more preferably 4,000, even more preferably 3,500, and particularly preferably 3,000.

[0144] [[A2] Compound synthesis method] The compound [A2] can be synthesized, for example, in the same manner as in the synthesis scheme exemplified in the synthesis method for the compound [A1] described above. Note that the compound represented by formula (a-3) in the synthesis scheme above is an example of the compound (A2-5), and the compound represented by formula (a-4) is an example of the compound (A2-2). [Example]

[0145] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0146] <Synthesis of Compound [A]> The compounds represented by the following formulas (a-1) to (a-8), (A-1) to (A-12), (ca-1), and (CA-1) (hereinafter also referred to as "compounds (a-1) to (a-8), (A-1) to (A-12), (ca-1), and (CA-1)") were synthesized by the following procedure.

[0147] [ka]

[0148] [ka]

[0149] [ka]

[0150] [ka]

[0151] [ka]

[0152] [Synthesis Example 1] (Synthesis of Compound (a-1)) A reaction vessel was charged with 20.0 g of 2-phenylethynylfluorene and 200 g of 1,4-dioxane under a nitrogen atmosphere and dissolved at 50°C. Next, 1.28 g of octacarbonyl dicobalt was added, and the mixture was heated to 110°C and reacted for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, and 600 g of methanol and 60.0 g of water were added to obtain a precipitate. The obtained precipitate was collected with filter paper, washed with a large amount of methanol, and dried to obtain compound (a-1). The molecular weight of compound (a-1) was 799.

[0153] [Synthesis Example 2] (Synthesis of Compound (a-2)) A reaction vessel was charged with 15.0 g of the compound (a-1) and 760 g of dichloromethane under a nitrogen atmosphere. The mixture was dissolved at room temperature and then cooled to 0°C. A solution of 60.9 g of anhydrous iron (III) chloride dissolved in 380 g of nitromethane was then added dropwise. The mixture was allowed to react at 0°C for 2 hours, then heated to 20°C and allowed to react for another 2 hours. After the reaction was completed, 1,140 g of methanol was added to obtain a precipitate. The obtained precipitate was collected using filter paper, washed with a large amount of methanol and tetrahydrofuran (hereinafter also referred to as "THF"), and dried to obtain compound (a-2). The molecular weight of compound (a-2) was 787.

[0154] [Synthesis Example 3] (Synthesis of Compound (a-3)) In a nitrogen atmosphere, 20.0 g of bis(2-fluorenyl)acetylene and 600 g of 1,4-dioxane were added to a reaction vessel and stirred at 50°C. After that, 3.85 g of octacarbonyl dicobalt was added, and the mixture was heated to 110°C and reacted for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, and 600 g of methanol and 60.0 g of water were added to obtain a precipitate. The obtained precipitate was collected with filter paper, washed with a large amount of a 50 / 50 mass% THF / hexane solution, and dried to obtain compound (a-3). The molecular weight of compound (a-3) was 1,063.

[0155] [Synthesis Example 4] (Synthesis of Compound (a-4)) Compound (a-4) was obtained in the same manner as in Synthesis Example 2, except that 20.0 g of compound (a-3) was used instead of 15.0 g of compound (a-1). The molecular weight of compound (a-4) was 1,051.

[0156] [Synthesis Example 5] (Synthesis of Compound (a-5)) In a nitrogen atmosphere, 20.0 g of bis(2-fluorenyl)acetylene, 21.7 g of tetraphenylcyclopentadienone, and 125 g of sulfolane were added to a reaction vessel, stirred at 50°C, and then heated to 210°C and reacted for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, and 125 g of methanol and 50.0 g of water were added to obtain a precipitate. The obtained precipitate was recrystallized from toluene and dried to obtain compound (a-5). The molecular weight of compound (a-5) was 711.

[0157] [Synthesis Example 6] (Synthesis of Compound (a-6)) Compound (a-6) was obtained in the same manner as in Synthesis Example 2, except that 13.9 g of compound (a-5) was used instead of 15.0 g of compound (a-1). The molecular weight of compound (a-6) was 699.

[0158] [Synthesis Example 7] (Synthesis of Compound (A-1)) In a nitrogen atmosphere, 10.0 g of the compound (a-2), 14.7 g of t-butyl acrylate, and 162 g of THF were added to a reaction vessel and stirred. Then, 15.4 g of a 50% by mass aqueous solution of potassium hydroxide and 2.46 g of tetrabutylammonium bromide were added, and the mixture was allowed to react at 60°C for 4 hours. After the reaction was completed, the mixture was cooled to room temperature, and 162 g of methyl isobutyl ketone was added. After removing the aqueous phase, separation and extraction were performed using a 1% by mass aqueous solution of oxalic acid and water. The organic layer was poured into hexane and reprecipitated. The precipitate was collected using filter paper and dried to obtain compound (A-1). The molecular weight of compound (A-1) was 1,556.

[0159] [Synthesis Example 8] (Synthesis of Compound (A-2)) Compound (A-2) was obtained in the same manner as in Synthesis Example 7, except that 21.5 g of 2-(2-ethoxyethoxy)ethyl acrylate was used instead of 22.3 g of t-butyl acrylate. The molecular weight of compound (A-2) was 1,916.

[0160] [Synthesis Example 9] (Synthesis of Compound (A-3)) Compound (A-3) was obtained in the same manner as in Synthesis Example 7, except that 6.5 g of compound (a-4) was used instead of 10.0 g of compound (a-2). The molecular weight of compound (A-3) was 2,589.

[0161] [Synthesis Example 10] (Synthesis of Compound (A-4)) Compound (A-4) was obtained in the same manner as in Synthesis Example 7, except that 14.0 g of compound (a-6) was used instead of 10.0 g of compound (a-2). The molecular weight of compound (A-4) was 1,212.

[0162] [Synthesis Example 11] (Synthesis of Compound (A-5)) In a reaction vessel, 10.0 g of the compound (a-3), 200 g of THF, and 19.0 g of potassium t-butoxide were added under a nitrogen atmosphere and stirred at 60°C for 30 minutes. After cooling to -40°C, 20.1 g of propargyl bromide was added dropwise and allowed to react at 0°C for 2 hours. After completion of the reaction, 500 g of a 5% by mass aqueous solution of oxalic acid and 100 g of methyl isobutyl ketone were added. After removing the aqueous phase, separation and extraction with water was performed, and the organic layer was poured into hexane for reprecipitation. The precipitate was collected using filter paper and dried to obtain compound (A-5). The molecular weight of compound (A-5) was 1,520.

[0163] [Synthesis Example 12] (Synthesis of Compound (A-6)) Compound (A-6) was obtained in the same manner as in Synthesis Example 11, except that 14.0 g of compound (a-2) was used instead of 10.0 g of compound (a-3). The molecular weight of compound (A-6) was 1,015.

[0164] [Synthesis Example 13] (Synthesis of Compound (A-7)) In a nitrogen atmosphere, 10.0 g of the compound (a-3), 8.81 g of 3-ethynylbenzaldehyde, and 94.1 g of N-methylpyrrolidone were added to a reaction vessel and stirred. Then, 17.2 g of diazabicycloundecene was added and the mixture was reacted at 120°C for 24 hours. After the reaction was completed, 500 g of a 5% by mass aqueous solution of oxalic acid and 100 g of methyl isobutyl ketone were added. After removing the aqueous phase, separation and extraction with water were performed, and the organic layer was poured into hexane for reprecipitation. The precipitate was collected with filter paper and dried to obtain compound (A-7). The molecular weight of compound (A-7) was 1,736.

[0165] [Synthesis Example 13] (Synthesis of Compound (A-8)) In a nitrogen atmosphere, 10.0 g of the compound (a-1), 6.54 g of indole-3-carboxaldehyde, and 82.7 g of m-xylene were added to a reaction vessel and stirred. Then, 17.2 g of diazabicycloundecene was added and the mixture was reacted at 140°C for 24 hours. After the reaction was completed, 500 g of a 5% by mass aqueous solution of oxalic acid and 100 g of methyl isobutyl ketone were added. After removing the aqueous phase, separation and extraction with water were performed, and the organic layer was poured into hexane for reprecipitation. The precipitate was collected with filter paper and dried to obtain compound (A-8). The molecular weight of compound (A-8) was 1,180.

[0166] [Synthesis Example 14] (Synthesis of Compound (A-9)) Compound (A-9) was obtained in the same manner as in Synthesis Example 13, except that 6.76 g of piperonal was used instead of 6.54 g of indole-3-carboxaldehyde. The molecular weight of compound (A-9) was 1,195.

[0167] [Synthesis Example 15] (Synthesis of Compound (a-7)) A reaction vessel was charged with 10.0 g of 1,3,6,8-tetrabromopyrene, 33.86 g of 9H-fluorene-2-boronic acid pinacol, and 300 g of tetrahydrofuran under a nitrogen atmosphere. After stirring, 169 g of 20% by weight aqueous potassium carbonate solution and 1.28 g of [1,1'-bis(diphenylphosphino)ferrocene]palladium(II) dichloride dichloromethane adduct were added, heated to 70 °C, and reacted for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, and 300 g of methyl isobutyl ketone and 100 g of water were added to obtain a precipitate. The resulting precipitate was collected using filter paper, washed with a large amount of tetrahydrofuran, and dried to obtain compound (a-7). The molecular weight of compound (a-7) was 859.

[0168] [Synthesis Example 16] (Synthesis of Compound (a-8)) Compound (a-8) was obtained in the same manner as in Synthesis Example 15, except that 14.0 g of 1,6-dibromopyrene was used instead of 10.0 g of 1,3,6,8-tetrabromopyrene. The molecular weight of compound (a-8) was 531.

[0169] [Synthesis Example 17] (Synthesis of Compound (A-10)) Compound (A-10) was obtained in the same manner as in Synthesis Example 11, except that 23 g of compound (a-7) was used instead of 10.0 g of compound (a-3). The molecular weight of compound (A-10) was 1,163.

[0170] [Synthesis Example 18] (Synthesis of Compound (A-11)) Compound (A-11) was obtained in the same manner as in Synthesis Example 13, except that 10.0 g of compound (a-8) and 5.88 g of 3-ethynylbenzaldehyde were used instead of 10.0 g of compound (a-1) and 6.54 g of indole-3-carboxyaldehyde. The molecular weight of compound (A-11) was 755.

[0171] [Synthesis Example 19] (Synthesis of Compound (A-12)) In a nitrogen atmosphere, 10.0 g of the compound (a-3), 14.3 g of 1-formylpyrene, and 121.5 g of tetrahydrofuran were added to a reaction vessel and stirred. Then, 52.8 g of a 25% by mass aqueous solution of tetramethylammonium hydroxide and 1.82 g of tetrabutylammonium bromide were added, and the mixture was allowed to react at 60°C for 12 hours. After the reaction was completed, 500 g of a 5% by mass aqueous solution of oxalic acid and 100 g of methyl isobutyl ketone were added. After removing the aqueous phase, separation and extraction with water were performed, and the organic layer was poured into hexane for reprecipitation. The precipitate was collected using filter paper and dried to obtain compound (A-12). The molecular weight of compound (A-12) was 2,337.

[0172] Comparative Synthesis Example 1 (Synthesis of Compound (ca-1)) A reaction vessel was charged with 20.0 g of 2-acetylfluorene and 20.0 g of m-xylene under a nitrogen atmosphere and dissolved at 110°C. Next, 3.14 g of dodecylbenzenesulfonic acid was added, and the mixture was heated to 140°C and reacted for 16 hours. After the reaction was completed, the reaction solution was diluted with 80 g of xylene, cooled to 50°C, and poured into 500 g of methanol for reprecipitation. The resulting precipitate was washed with toluene, and the solid was collected on filter paper and dried to obtain compound (ca-1).

[0173] Comparative Synthesis Example 2 (Synthesis of Compound (CA-1)) In a nitrogen atmosphere, 10.0 g of the compound (ca-1), 18.8 g of propargyl bromide, and 50 g of toluene were added to a reaction vessel and stirred. Then, 25.2 g of 50% by mass aqueous sodium hydroxide and 1.7 g of tetrabutylammonium bromide were added, and the reaction was carried out at 92°C for 12 hours. The reaction solution was cooled to 50°C, and 25 g of tetrahydrofuran was added. After removing the aqueous phase, 50 g of 1% by mass aqueous oxalic acid was added to perform separation and extraction, followed by pouring into hexane and reprecipitation. The precipitate was collected using filter paper and dried to obtain compound (CA-1). The molecular weight of compound (CA-1) was 799.

[0174] <Preparation of Composition> The solvents [B] used in the preparation of the compositions are shown below.

[0175] [[B] Solvent] B-1: Propylene glycol monomethyl ether acetate B-2: Cyclohexanone

[0176] [Example 1-1] (Preparation of Composition (J-1)) 10 parts by mass of (A-1) as the compound [A] was dissolved in 90 parts by mass of (B-1) as the solvent [B]. The resulting solution was filtered through a membrane filter with a pore size of 0.1 μm to prepare composition (J-1).

[0177] [Examples 1-2 to 1-12 and Comparative Example 1-1] (Preparation of Compositions (J-2) to (J-12) and (CJ-1)) Compositions (J-2) to (J-12) and (CJ-1) were prepared in the same manner as in Example 1, except that the types and amounts of each component shown in Table 1 below were used.

[0178] [Table 1]

[0179] <Film formation> [Examples 2-1 to 2-12 and Comparative Example 2-1] The composition prepared above was applied onto a silicon wafer (substrate) by spin coating using a spin coater (Tokyo Electron Ltd.'s "LITHIUS Pro Z"), followed by heating at 400°C for 60 seconds in an air atmosphere and then cooling at 23°C for 600 seconds to obtain a substrate with a film having an average thickness of 200 nm.

[0180] <Evaluation> The etching resistance, heat resistance, and embeddability of the composition prepared in the above <Preparation of Composition> and the film-coated substrate obtained in the above <Formation of Film> were evaluated by the following methods. The evaluation results are shown in Table 2 below.

[0181] [Etching resistance] The film on the film-coated substrate was treated using an etching system (Tokyo Electron Limited, "TACTRAS") under the following conditions: CF4 / Ar = 110 / 440 sccm, PRESS = 30 MT, HF RF (plasma generation radio frequency power) = 500 W, LF RF (bias radio frequency power) = 3000 W, DCS = -150 V, RDC (gas center flow ratio) = 50%, and 30 seconds. The etching rate (nm / min) was calculated from the average thickness of the film before and after treatment. Next, the ratio relative to the etching rate of Comparative Example 2-1 was calculated as a standard and used as a measure of etching resistance. Etching resistance was evaluated as "A" (very good) when the ratio was less than 0.90, "B" (good) when it was 0.90 or more but less than 1.00, and "C" (poor) when it was 1.00 or more. In Table 2 below, "*" indicates that this is the evaluation standard for etching resistance.

[0182] [Heat resistance] The film-coated substrate was further heated in a nitrogen atmosphere at 450°C for 600 seconds, and then cooled at 23°C for 60 seconds. The average thickness of the film was measured before and after this treatment. The average thickness of the film before treatment was designated X0, and the average thickness of the film after treatment was designated X. The absolute value of the value obtained by (X-X0) x 100 / X0 was calculated as the film thickness change rate (%). Heat resistance was evaluated as "A" (very good) when the film thickness change rate was less than 2%, "B" (good) when it was 2% or more but less than 5%, and "C" (poor) when it was 5% or more.

[0183] [Embeddability] The composition was applied by spin coating using the spin coater to a substrate on which a line-and-space pattern of 100 nm in depth and width had been formed. The spin coater rotation conditions were the same as those for obtaining a substrate with a film of 200 nm average thickness. The substrate was then heated at 400°C for 60 seconds in an air atmosphere, followed by cooling at 23°C for 60 seconds. The cross-sectional shape of the substrate was observed using a scanning electron microscope (Hitachi High-Technologies Corporation, S-4800) to evaluate the embeddability. The embeddability was evaluated as "A" (good) if the film was embedded to the bottom of the space pattern on the substrate, and "B" (poor) if the film was not embedded to the bottom of the space pattern.

[0184] [Table 2]

[0185] The results in Table 2 show that the films formed from the compositions of the examples were superior in etching resistance and heat resistance to the films formed from the compositions of the comparative examples, and that the compositions of the examples had the same embedding ability as the compositions of the comparative examples. [Industrial Applicability]

[0186] The composition of the present invention can form a film having excellent etching resistance, heat resistance, and embedding ability. The resist underlayer film of the present invention has excellent etching resistance, heat resistance, and embedding ability. The method for forming a resist underlayer film of the present invention can form a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability. The method for producing a patterned substrate of the present invention can form a resist underlayer film having excellent etching resistance, heat resistance, and embedding ability, thereby obtaining a well-patterned substrate. The compound of the present invention can be suitably used as a component of a composition for forming a resist underlayer film. Therefore, these compounds can be suitably used in the production of semiconductor devices, which are expected to become even more miniaturized in the future.

Claims

1. A step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate. Equipped with The composition for forming a resist underlayer film, Compounds represented by the following formulas (A1-1) to (A1-8), Solvent and A method for forming a resist underlayer film comprising the steps of: 【Chemical 1】 【Chemistry 2】 (In formulas (A1-1) to (A1-8), X is a group represented by the following formula (i), (ii), (iii), or (iv).) 【Chemistry 3】 (In formula (i), R 1 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 2 is a monovalent organic group having 1 to 20 carbon atoms. In formula (ii), R 3 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 4 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iii), R 5 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iv), R 6 is a monovalent organic group having 1 to 20 carbon atoms. The above R 1 , R 2 , R 3 , R 4 , R 5 and R 6 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (x-1) to (x-12) below is a group represented by the formula (x-1) to (x-12). 【Chemistry 4】 (In formulas (x-1) to (x-12), ** represents the bonding site to the carbon atom or nitrogen atom in formula (i), (ii), (iii), or (iv) above.)

2. a step of directly or indirectly applying a composition for forming a resist underlayer film to a substrate; a step of forming a resist pattern directly or indirectly on the resist underlayer film formed by the coating step; a step of performing etching using the resist pattern as a mask; Equipped with The composition for forming a resist underlayer film, Compounds represented by the following formulas (A1-1) to (A1-8), Solvent and A method for producing a patterned substrate comprising: 【Chemistry 5】 【Chemistry 6】 (In formulas (A1-1) to (A1-8), X is a group represented by the following formula (i), (ii), (iii), or (iv).) 【Chemistry 7】 (In formula (i), R 1 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 2 is a monovalent organic group having 1 to 20 carbon atoms. In formula (ii), R 3 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 4 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iii), R 5 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iv), R 6 is a monovalent organic group having 1 to 20 carbon atoms. The above R 1 , R 2 , R 3 , R 4 , R 5 and R 6 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (x-1) to (x-12) below is a group represented by the formula (x-1) to (x-12). 【Chemistry 8】 (In formulas (x-1) to (x-12), ** represents the bonding site to the carbon atom or nitrogen atom in formula (i), (ii), (iii), or (iv) above.)

3. Before the resist pattern forming step, A step of forming a silicon-containing film directly or indirectly on the resist underlayer film formed by the coating step. The method for manufacturing a patterned substrate according to claim 2 , further comprising:

4. Compounds represented by the following formulas (A1-1) to (A1-8), Solvent and A composition for forming a resist underlayer film comprising: 【Chemistry 9】 【Chemistry 10】 (In formulas (A1-1) to (A1-8), X is a group represented by the following formula (i), (ii), (iii), or (iv).) 【Chemistry 11】 (In formula (i), R 1 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 2 is a monovalent organic group having 1 to 20 carbon atoms. In formula (ii), R 3 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 4 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iii), R 5 is a monovalent organic group having 1 to 20 carbon atoms. In formula (iv), R 6 is a monovalent organic group having 1 to 20 carbon atoms. The above R 1 , R 2 , R 3 , R 4 , R 5 and R 6 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (x-1) to (x-12) below is a group represented by the formula (x-1) to (x-12). 【Chemistry 12】 (In formulas (x-1) to (x-12), ** represents the bonding site to the carbon atom or nitrogen atom in formula (i), (ii), (iii), or (iv) above.)

5. 5. The composition for forming a resist underlayer film according to claim 4, wherein X is a group represented by the above formula (i) or (ii).

Citation Information

Patent Citations

  • Base layer film forming material for multilayer resist process, and wiring formation method using the same

    JP2004177668A

  • Composition for formation of resist underlayer film which contains fullerene derivative

    WO2011108365A1

  • Composition for forming resist underlayer film, resist underlayer film, method for producing same, and method for producing patterned substrate