(Meth)acrylic copolymer, (meth)acrylic copolymer composition and ink
The (meth)acrylic copolymer composition addresses solubility and stability issues in water-based inks by incorporating specific structural units and polymerization methods, resulting in a formulation with enhanced alkaline water solubility and film printing performance.
Patent Information
- Application Number
- JP2022563580
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-18
- Filing Date
- 2021-08-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-06
AI Technical Summary
Existing (meth)acrylic copolymers for water-based inks face issues with low solubility in alkaline water, poor storage stability, and inadequate hiding properties in film printing, often requiring high-temperature processes that increase energy consumption and residual solvent content.
A (meth)acrylic copolymer composition comprising structural units derived from (meth)acrylic acid alkyl esters, acid group-containing vinyl compounds, and trifunctional or higher functional mercaptans, with optional monofunctional or bifunctional mercaptan structures, designed to enhance solubility and stability, and a process involving suspension or bulk polymerization followed by dehydration and drying to achieve particulate form.
The (meth)acrylic copolymer exhibits excellent solubility in alkaline water, improved storage stability, and superior hiding properties in film printing, reducing volatile organic compounds and enhancing productivity.
Smart Images

Figure 0007589748000001 
Figure 0007589748000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a (meth)acrylic copolymer, a (meth)acrylic copolymer composition, and an ink. This application claims priority based on Patent Application No. 2020-192003, filed with the Japan Patent Office on November 18, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] Unlike solvent-based inks, water-based inks (also called aqueous inks) can reduce the amount of volatile organic compounds (VOCs) and can reduce the risk of fire and toxicity such as mutagenicity. For this reason, water-based inks are widely used in applications such as gravure printing. In particular, (meth)acrylic polymers and (meth)acrylic copolymers that contain structural units derived from (meth)acrylic acid alkyl esters and structural units derived from (meth)acrylic acid are widely used in water-based ink applications due to their high transparency and good pigment color development.
[0003] (Meth)acrylic polymers and (meth)acrylic copolymers for water-based inks are required to have good solubility in alkaline water, as well as low total VOCs when dissolved, ink storage stability, and good hiding power when printed on film.
[0004] Patent Document 1 describes a method for producing a water-dilutable coating resin by condensing a polycarboxylic acid resin and a polyol resin produced by solution polymerization using a polyfunctional mercaptan in a solvent different from the polymerization solvent, and then neutralizing the resulting mixture with an amine at 95°C and dispersing it in deionized water. Patent Document 2 describes a method for obtaining an aqueous pigment dispersion with high storage stability by introducing a hydrophobic moiety and a hydrophilic moiety into a multifunctional mercaptan prepared in a solution. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 04-304277 [Patent Document 2] International Publication No. 2019 / 065604 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the method described in Patent Document 1 requires repeated devolatilization of the solvent. In addition, the resin is condensed or melted at a high temperature of about 95°C before being neutralized with an amine, which results in low solubility of the resin in alkaline water. In addition, the total amount of energy required to obtain an aqueous dispersion is large, and there is a problem that the solvent used in the polymerization and condensation steps remains in the final composition.
[0007] The method of Patent Document 2 requires a long polymerization process and poor productivity because the hydrophobic and hydrophilic parts are introduced through multiple polymerization steps. In addition, the (meth)acrylic copolymer obtained in the polymerization step needs to be neutralized with alkali at a high temperature of 70°C. This causes a problem that the (meth)acrylic copolymer has low solubility in alkaline water.
[0008] The present invention aims to provide a (meth)acrylic copolymer having good solubility in alkaline water and having good storage stability of the ink and good hiding power in film printing; a (meth)acrylic copolymer composition containing the (meth)acrylic copolymer; and an ink containing the (meth)acrylic copolymer composition. [Means for solving the problem]
[0009] The present invention has the following aspects. [1] A (meth)acrylic copolymer which is a particulate solid and has a structural unit derived from a (meth)acrylic acid alkyl ester in which the alkyl group has 1 to 8 carbon atoms, a structural unit derived from an acid group-containing vinyl compound, and a chemical structure derived from a tri- or higher functional mercaptan. [2] A (meth)acrylic copolymer having a structural unit derived from a (meth)acrylic acid alkyl ester, the alkyl group of which has 1 to 8 carbon atoms, a structural unit derived from an acid group-containing vinyl compound, and a chemical structure derived from a tri- or higher functional mercaptan, and further having one or more chemical structures selected from the group consisting of chemical structures derived from monofunctional mercaptans and chemical structures derived from difunctional mercaptans. [3] The (meth)acrylic copolymer according to [1] or [2], wherein the (meth)acrylic copolymer has a second-order glass transition temperature of 35° C. or higher. [4] The (meth)acrylic copolymer according to any one of [1] to [3], further comprising a structural unit derived from a compound having two or more polymerizable double bonds. [5] The (meth)acrylic copolymer of any one of [1], [3], and [4], further having one or more chemical structures selected from the group consisting of chemical structures derived from monofunctional mercaptans and chemical structures derived from difunctional mercaptans. [6] The (meth)acrylic copolymer according to any one of [1] to [5], wherein the (meth)acrylic copolymer has a mass average particle size of 20 to 2000 μm. [7] The (meth)acrylic copolymer according to any one of [1] to [6], wherein the (meth)acrylic copolymer has a water content of 0.01 to 10 mass %. [8] The (meth)acrylic copolymer according to any one of [1] to [7], wherein the (meth)acrylic copolymer has an acid value of 20 to 140 mgKOH / g. [9] The (meth)acrylic copolymer according to any one of [1] to [8], wherein the (meth)acrylic copolymer has a weight average molecular weight of 15,000 to 80,000.
[10] A (meth)acrylic copolymer composition comprising the (meth)acrylic copolymer according to any one of [1] to [9], water, and a basic compound.
[11] The (meth)acrylic copolymer composition of
[10] , further comprising a pigment.
[12] An ink comprising the (meth)acrylic copolymer composition of
[10] or
[11] . Effect of the Invention
[0010] According to the present invention, there can be provided a (meth)acrylic copolymer which has good solubility in alkaline water and exhibits good storage stability of the ink and good hiding power in film printing, a (meth)acrylic copolymer composition containing the (meth)acrylic copolymer, and an ink containing the (meth)acrylic copolymer composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from the spirit of the present invention.
[0012] In this specification, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid. "(meth)acrylic" is a general term for acrylic and methacrylic. "(meth)acrylic copolymer" is, for example, a copolymer having at least one of an acryloyl group and a methacryloyl group. In this specification, "(meth)acrylate" is a general term for acrylate and methacrylate. In this specification, the ratio of each constituent unit of the (meth)acrylic copolymer and the ratio of the chemical structure derived from mercaptan refer to values calculated from the mass ratio of each monomer and mercaptan used in the polymerization raw materials. In this specification, "room temperature" means a temperature within the range of 23°C ± 2°C unless otherwise specified.
[0013] [(Meth)acrylic copolymer] <First aspect of (meth)acrylic copolymer> The (meth)acrylic copolymer according to the first aspect of the present invention has a structural unit derived from a (meth)acrylic acid alkyl ester having an alkyl group of 1 to 8 carbon atoms (hereinafter also referred to as "monomer (a)"), a structural unit derived from an acid group-containing vinyl compound (hereinafter also referred to as "monomer (b)"), and a chemical structure derived from a tri- or higher functional mercaptan. The (meth)acrylic copolymer of the first embodiment preferably further has one or more chemical structures selected from the group consisting of chemical structures derived from monofunctional mercaptans and chemical structures derived from difunctional mercaptans. The (meth)acrylic copolymer may further have a structural unit derived from a monomer other than the monomers (a) and (b) (hereinafter also referred to as "monomer (c)").
[0014] <(Meth)acrylic copolymer according to the second embodiment> The (meth)acrylic copolymer of the second aspect of the present invention has a structural unit derived from a monomer (a), a structural unit derived from a monomer (b), and a chemical structure derived from a trifunctional or higher functional mercaptan, and further has one or more chemical structures selected from the group consisting of a chemical structure derived from a monofunctional mercaptan and a chemical structure derived from a difunctional mercaptan. The (meth)acrylic copolymer of the second aspect may further have a structural unit derived from a monomer (c).
[0015] <(Meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms> The (meth)acrylic copolymers according to the first and second aspects of the present invention have structural units derived from a (meth)acrylic acid alkyl ester having an alkyl group of 1 to 8 carbon atoms, i.e., structural units derived from monomer (a). Examples of the monomer (a) in the (meth)acrylic copolymer of the first and second embodiments include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate. Among these, methyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl acrylate are preferred because they provide a (meth)acrylic copolymer with better solubility in alkaline water and are easily available. These may be used alone or in combination of two or more.
[0016] The proportion of the constituent units derived from the monomer (a) in the (meth)acrylic copolymer of the first and second embodiments is preferably 60 to 97% by mass, more preferably 80 to 95% by mass, based on 100% by mass of the total of the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b). The lower and upper limits of these numerical ranges can be arbitrarily combined. When the proportion of the constituent units derived from the monomer (a) is within the above range, the film-forming properties and water resistance of the ink are good.
[0017] <Acid group-containing vinyl compound> The (meth)acrylic copolymers according to the first and second aspects of the present invention have a constituent unit derived from an acid group-containing vinyl compound, that is, a constituent unit derived from the monomer (b). Examples of the monomer (b) include vinyl compounds having an acid group such as a carboxylic acid or sulfonic acid group. Specific examples of the vinyl compound having a carboxylic acid group in the (meth)acrylic copolymer of the first embodiment and the second embodiment include monobasic acids such as (meth)acrylic acid and crotonic acid; dibasic acids such as fumaric acid, maleic acid and itaconic acid; and partial esters of these dibasic acids. Specific examples of vinyl compounds having a sulfonic acid group include vinyl sulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid. Among these, vinyl compounds having a carboxylic acid group are preferred, and (meth)acrylic acid is more preferred, in terms of improving the water solubility of the (meth)acrylic copolymer. These may be used alone or in combination of two or more.
[0018] The proportion of the constituent units derived from the monomer (b) in the (meth)acrylic copolymer of the first and second embodiments is preferably 3 to 40 mass%, more preferably 5 to 20 mass%, in the total of 100 mass% of the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b). The lower and upper limits of these numerical ranges can be arbitrarily combined. When the proportion of the structural units derived from the monomer (b) is within the above range, the (meth)acrylic copolymer has better solubility in alkaline water and other solvents.
[0019] The total proportion of the constituent units derived from monomer (a) and the constituent units derived from monomer (b) in the (meth)acrylic copolymer of the first and second embodiments is preferably 70 to 99.9% by mass, more preferably 80 to 99% by mass, and even more preferably 85 to 95% by mass, based on the total mass of all the constituent units constituting the (meth)acrylic copolymer. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the total proportion of the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b) is within the above range, the solubility in alkaline water is extremely good. In this specification, the total mass of all the constituent units constituting the (meth)acrylic copolymer of the first embodiment and the second embodiment includes the proportion of the chemical structure derived from metacaptan, which will be described later.
[0020] <Mercaptan> The (meth)acrylic copolymers of the first and second embodiments have a chemical structure derived from a tri- or higher functional mercaptan. Although the details will be described later, by using a tri- or higher functional mercaptan as a chain transfer agent in the polymerization reaction when producing the (meth)acrylic copolymer of the first embodiment and the second embodiment, the tri- or higher functional mercaptan serves as the initiation point of polymerization, and a chemical structure derived from the tri- or higher functional mercaptan is introduced into the (meth)acrylic copolymer.
[0021] Trifunctional or higher mercaptans are compounds that have three or more mercapto groups in a single molecule. Examples of trifunctional or higher mercaptans in the (meth)acrylic copolymers of the first and second embodiments include 1,2,3-trimercaptopropane, 2,2-bis(mercaptomethyl)-1-mercaptobutane, 1,2,3,4-tetramercaptobutane, 2,2-bis(mercaptomethyl)-1,3-dimercaptopropane, glycerin tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), and the like. nate), dipentaerythritol hexakis(3-mercaptopropionate), glycerin tris(thioglycolate), trimethylolpropane tris(thioglycolate), pentaerythritol tetrakis(thioglycolate), dipentaerythritol hexakis(thioglycolate), trimethylolpropane tris(2-mercaptobutyrate), pentaerythritol tetrakis(2-mercaptobutyrate), dipentaerythritol hexakis(2-mercaptobutyrate), and the like. Among these, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), and pentaerythritol tetrakis(thioglycolate) are preferred, since they provide a better solubility of the (meth)acrylic copolymer in alkaline water and are easily available. These may be used alone or in combination of two or more.
[0022] The ratio of the trifunctional or higher mercaptan-derived chemical structure in the (meth)acrylic copolymer of the first and second embodiments is preferably 0.1 to 20 parts by mass, more preferably 1 to 6 parts by mass, relative to 100 parts by mass of the total of the structural units derived from all monomers constituting the (meth)acrylic copolymer. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the ratio of the chemical structure derived from a trifunctional or higher mercaptan is equal to or higher than the lower limit, the solubility of the (meth)acrylic copolymer in alkaline water tends to be better. When the ratio of the chemical structure derived from a trifunctional or higher mercaptan is equal to or lower than the upper limit, the odor of the (meth)acrylic copolymer is suppressed.
[0023] The (meth)acrylic copolymer of the first embodiment preferably further has one or more chemical structures selected from the group consisting of a monofunctional mercaptan-derived chemical structure and a bifunctional mercaptan-derived chemical structure in addition to the trifunctional or higher mercaptan-derived chemical structure. When the (meth)acrylic copolymer of the first embodiment further has one or more chemical structures selected from the group consisting of a monofunctional mercaptan-derived chemical structure and a bifunctional mercaptan-derived chemical structure, the viscosity when dissolved in alkaline water is reduced, making it easier to incorporate pigments and the like.
[0024] The (meth)acrylic copolymer of the second aspect has, in addition to the chemical structure derived from a trifunctional or higher mercaptan, one or more chemical structures selected from the group consisting of a chemical structure derived from a monofunctional mercaptan and a chemical structure derived from a bifunctional mercaptan. Therefore, the (meth)acrylic copolymer of the second aspect has a low viscosity when dissolved in alkaline water, making it easy to incorporate pigments and the like.
[0025] Monofunctional mercaptans are compounds that have one mercapto group in a single molecule. Examples of the monofunctional mercaptan in the (meth)acrylic copolymer of the first embodiment and the second embodiment include n-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, n-butyl mercaptan, thioglycolic acid, 3-mercaptopropionic acid, 2-mercaptoethanol, 2-ethylhexyl 3-mercaptopropionate, 2-ethylhexyl thioglycolate, isooctyl 3-mercaptopropionate, isooctyl thioglycolate, and 2-methoxybutyl 3-mercaptopropionate. These may be used alone or in combination of two or more.
[0026] The proportion of the monofunctional mercaptan-derived chemical structure in the (meth)acrylic copolymer of the first and second embodiments is preferably 0.1 to 20 parts by mass, more preferably 1 to 6 parts by mass, relative to 100 parts by mass of the total of the structural units derived from all monomers constituting the (meth)acrylic copolymer. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the proportion of the chemical structure derived from the monofunctional mercaptan is equal to or greater than the lower limit, the solubility of the (meth)acrylic copolymer in alkaline water tends to be better. If the proportion of the chemical structure derived from the monofunctional mercaptan is equal to or less than the upper limit, the odor of the (meth)acrylic copolymer is suppressed.
[0027] A difunctional mercaptan is a compound that has two mercapto groups in a single molecule. Examples of the bifunctional mercaptan in the (meth)acrylic copolymer of the first and second embodiments include 1,4-dimercaptobutane, 3-oxo-1,5-pentanedithiol, 3-thia-1,5-pentanedithiol, ethylene glycol bis(3-mercaptopropionate), and 1,4-butanediol bis(thioglycolate). These may be used alone or in combination of two or more.
[0028] The ratio of the bifunctional mercaptan-derived chemical structure in the (meth)acrylic copolymer of the first and second embodiments is preferably 0.1 to 20 parts by mass, more preferably 1 to 6 parts by mass, relative to 100 parts by mass of the total of the structural units derived from all monomers constituting the (meth)acrylic copolymer. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the ratio of the bifunctional mercaptan-derived chemical structure is equal to or greater than the lower limit, the (meth)acrylic copolymer tends to have better solubility in alkaline water. If the ratio of the bifunctional mercaptan-derived chemical structure is equal to or less than the upper limit, the odor of the (meth)acrylic copolymer is suppressed.
[0029] <Other monomers> The (meth)acrylic copolymer of the first and second embodiments may further have a constituent unit derived from another monomer (monomer (c)) in addition to the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b). Examples of the monomer (c) in the (meth)acrylic copolymer of the first and second embodiments include a compound having one polymerizable double bond (hereinafter also referred to as "monomer (c1)") and a compound having two or more polymerizable double bonds (hereinafter also referred to as "monomer (c2)"). Among these, the monomer (c) is preferably monomer (c2). That is, the (meth)acrylic copolymer preferably further has a constituent unit derived from monomer (c2) in addition to the constituent units derived from monomer (a) and monomer (b).
[0030] Examples of the monomer (c1) in the (meth)acrylic copolymer of the first and second embodiments include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, o-methoxystyrene, m-methoxyethylene, p-methoxystyrene, 4-(tert-butyl)styrene, p-(tert-butoxy)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, phenyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, stearyl (meth)acrylate, and lauryl (meth)acrylate. These may be used alone or in combination of two or more.
[0031] The proportion of the constituent units derived from the monomer (c1) in the (meth)acrylic copolymer of the first and second embodiments is preferably 0.1 to 20 parts by mass, more preferably 1 to 6 parts by mass, per 100 parts by mass of the total of the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b). The lower and upper limits of these numerical ranges can be arbitrarily combined. When the ratio of the constituent units derived from the monomer (c1) is equal to or greater than the lower limit, the storage stability of the ink tends to be better. When the ratio of the constituent units derived from the monomer (c1) is equal to or less than the upper limit, the viscosity of the ink can be reduced, and handling during printing becomes easier.
[0032] Examples of the monomer (c2) in the (meth)acrylic copolymer of the first and second aspects include ethylene glycol di(meth)acrylate, 1,2-propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,4-cyclohexanedimethanol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,3-propylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and the like. acrylate, pentaerythritol tetra(meth)acrylate, bisphenol A di(meth)acrylate, 2,2-bis{4-[2-(acryloyloxy)ethoxy)]phenyl}propane, 2,2-bis{4-[2-(methacryloyloxy)ethoxy)]phenyl}propane, tricyclodecane dimethanol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, glycerin tri(meth)acrylate, ethoxy-modified isocyanuric acid tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-divinylbenzene, and 1,3,5-trivinylbenzene. Among these, ethylene glycol diacrylate, 1,6-hexanediol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate are preferred because they have a low viscosity when dissolved in alkaline water and can be easily incorporated with pigments and the like. These may be used alone or in combination of two or more.
[0033] The proportion of the constituent units derived from the monomer (c2) in the (meth)acrylic copolymer of the first and second embodiments is preferably 0.1 to 20 parts by mass, more preferably 1 to 6 parts by mass, per 100 parts by mass of the total of the constituent units derived from the monomer (a) and the constituent units derived from the monomer (b). The lower and upper limits of these numerical ranges can be arbitrarily combined. When the ratio of the constituent units derived from the monomer (c2) is equal to or greater than the lower limit, the storage stability of the ink tends to be better. When the ratio of the constituent units derived from the monomer (c2) is equal to or less than the upper limit, the viscosity of the ink can be reduced, and handling during printing becomes easy.
[0034] <Physical Properties> The (meth)acrylic copolymer of the first embodiment is solid at room temperature. Since the (meth)acrylic copolymer of the first embodiment is solid at room temperature, it can reduce VOCs when dissolved in alkaline water. In addition, it is possible to suppress the increase in bulk compared to the state where it is dissolved in water (aqueous solution) or dispersed in water (dispersion), so it is also suitable for transportation and storage. The (meth)acrylic copolymer of the second embodiment is also preferably solid at room temperature. When the (meth)acrylic copolymer of the second embodiment is solid at room temperature, it can reduce VOCs when dissolved in alkaline water. In addition, it is possible to suppress the increase in bulk compared to the state where it is dissolved in water (aqueous solution) or dispersed in water (dispersion), so it is also suitable for transportation and storage. Specific examples of the shape of the solid (meth)acrylic copolymer include powder, plate, crushed pieces, spheres, particles, granules, pellets, etc. Among these, powder, crushed pieces, spheres, particles, and granules are preferred because they are easy to handle when dissolved in a solvent or alkaline water. The (meth)acrylic copolymers of the first and second embodiments can be easily dissolved in water or a mixed solvent of water and an auxiliary solvent described below by neutralizing them with a basic compound described below.
[0035] The second glass transition temperature (Tg) of the (meth)acrylic copolymer of the first and second aspects is preferably 35° C. or higher, more preferably 40° C. or higher, and even more preferably 45° C. or higher. The second glass transition temperature (Tg) of the (meth)acrylic copolymer of the first and second aspects is preferably 70° C. or lower, more preferably 60° C. or lower, and even more preferably 55° C. or lower. These lower and upper limits can be combined in any combination. When the second glass transition temperature (Tg) of the (meth)acrylic copolymer of the first embodiment and the second embodiment is within the above range, aggregation between copolymer particles is suppressed when dissolved in alkaline water, and the solubility in alkaline water is improved. The second glass transition temperature (Tg) of the (meth)acrylic copolymer of the first embodiment and the second embodiment can be measured using a differential scanning calorimeter (DSC), and the specific measurement method is as described in the Examples section.
[0036] The mass average particle size of the (meth)acrylic copolymer of the first and second aspects is preferably 20 to 2000 μm, more preferably 50 to 850 μm, further preferably 80 to 700 μm, and particularly preferably 150 to 600 μm. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the mass average particle size of the (meth)acrylic copolymer is equal to or larger than the lower limit, the blending process becomes easy, and when the mass average particle size of the (meth)acrylic copolymer is equal to or smaller than the upper limit, the time required for dissolving in alkaline water is shortened. The mass average particle size of the (meth)acrylic copolymer can be calculated by shaking 20 g of the granular resin for 5 minutes and classifying it using a standard sieve.
[0037] The water content of the (meth)acrylic copolymer of the first and second aspects is preferably 0.01 to 10 mass%, more preferably 0.02 to 8.0 mass%, further preferably 0.1 to 5.0 mass%, particularly preferably 0.5 to 5.0 mass%, based on the total mass of the acrylic copolymer. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the water content of the (meth)acrylic copolymer is equal to or higher than the lower limit, the solubility in alkaline water is good. If the water content of the (meth)acrylic copolymer is equal to or lower than the upper limit, the water resistance of the printed matter is high. If the water content of the (meth)acrylic copolymer is within the above range, the copolymer is easy to handle when a particulate (meth)acrylic copolymer is obtained. A specific method for measuring the water content of the (meth)acrylic copolymer is as described in the Examples section.
[0038] The acid value of the (meth)acrylic copolymer of the first and second aspects is preferably 20 to 140 mgKOH / g, more preferably 50 to 100 mgKOH / g, and even more preferably 55 to 90 mgKOH / g. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the acid value of the (meth)acrylic copolymer is equal to or greater than the lower limit, the solubility in alkaline water is improved. If the acid value of the (meth)acrylic copolymer is equal to or less than the upper limit, the amount of basic compound required for neutralization and dissolution can be reduced, and the water resistance of the printed matter is improved. The acid value of the (meth)acrylic copolymer means the mass of potassium hydroxide required to neutralize 1 g of the (meth)acrylic copolymer, expressed in milligrams. The acid value of the (meth)acrylic copolymer of the first and second embodiments can be measured by neutralization titration with a potassium hydroxide solution based on the discoloration point of phenolphthalein. The specific measurement method is as described in the Examples section.
[0039] The weight average molecular weight (Mw) of the (meth)acrylic copolymer of the first embodiment and the second embodiment is preferably 15000 to 80000, more preferably 15000 to 60000, further preferably 20000 to 60000, particularly preferably 25000 to 60000, and most preferably 25000 to 40000. The lower limit and upper limit of these numerical ranges can be arbitrarily combined. When the weight average molecular weight of the (meth)acrylic copolymer is equal to or greater than the lower limit, the storage stability of the ink tends to be better.When the weight average molecular weight of the (meth)acrylic copolymer is equal to or less than the upper limit, the viscosity of the ink tends to be low, and the film-forming property tends to be good. The weight average molecular weight (Mw) of the (meth)acrylic copolymer of the first and second aspects is a weight average molecular weight (polystyrene equivalent) measured by gel permeation chromatography (GPC). The specific measurement method is as described in the Examples section.
[0040] The number average molecular weight (Mn) of the (meth)acrylic copolymer of the first aspect and the second aspect is preferably 5000 to 120000, more preferably 8000 to 80000, further preferably 12000 to 70000, particularly preferably 15000 to 60000, and most preferably 20000 to 50000. The lower limit and upper limit of these numerical ranges can be arbitrarily combined. When the number average molecular weight of the (meth)acrylic copolymer is equal to or greater than the lower limit, the storage stability of the ink tends to be better. When the number average molecular weight of the (meth)acrylic copolymer is equal to or less than the upper limit, the viscosity of the ink tends to be lower and the film-forming property tends to be better. The number average molecular weight (Mn) of the (meth)acrylic copolymer of the first and second aspects is a number average molecular weight (polystyrene equivalent) measured by gel permeation chromatography (GPC). The specific measurement method is as described in the Examples section.
[0041] <Manufacturing method> The (meth)acrylic copolymer of the first and second embodiments can be produced by a known polymerization method such as bulk polymerization, suspension polymerization, emulsion polymerization, etc. Among these polymerization methods, bulk polymerization and suspension polymerization are preferred because they tend to produce a powder, spherical, or particulate copolymer that is easy to handle.
[0042] <Suspension polymerization method> The method for producing the (meth)acrylic copolymer by suspension polymerization according to the first and second embodiments preferably includes a suspension polymerization step, a first dehydration step, a washing step, a second dehydration step, and a drying step.
[0043] (Suspension polymerization process) The suspension polymerization step is a step in which the above-mentioned monomer (a) and monomer (b), and optionally monomer (c), are dispersed in water and polymerized in the presence of a trifunctional or higher mercaptan to obtain the (meth)acrylic copolymer of the first embodiment and the second embodiment. A known method can be used for the suspension polymerization. For example, the suspension polymerization method includes a method in which the monomer (a) and the monomer (b), and optionally the monomer (c), are polymerized in water in the presence of a polymerization auxiliary in a reactor having a polymerization temperature control function and a stirring function.
[0044] Examples of polymerization aids that can be used in the production of the (meth)acrylic copolymer of the first and second embodiments include polymerization initiators, chain transfer agents, dispersants, dispersion aids, etc. However, at least the above-mentioned trifunctional or higher mercaptan is used as the chain transfer agent. By using a tri- or higher functional mercaptan as the polymerization auxiliary, the (meth)acrylic copolymer of the first embodiment and the second embodiment having a chemical structure derived from a tri- or higher functional mercaptan can be obtained.
[0045] Examples of polymerization initiators that can be used in the production of the (meth)acrylic copolymers of the first and second embodiments include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), benzoyl peroxide, lauroyl peroxide, tert-butylperoxy-2-ethylhexanoate, tert-amylhydroxy-2-ethylhexanoate, tert-hexylperoxy-2-ethylhexanoate, and 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate. These may be used alone or in combination of two or more.
[0046] As the chain transfer agent that can be used in the production of the (meth)acrylic copolymer of the first and second embodiments, a mercaptan having at least three functionalities is used. As the chain transfer agent, in addition to the trifunctional or higher functional mercaptan, at least one of the above-mentioned monofunctional mercaptan and difunctional mercaptan may be used in combination. Furthermore, in addition to these mercaptans, diphenyl disulfide, dibenzyl disulfide, and α-methylstyrene dimer may be used in combination. These may be used alone or in combination of two or more.
[0047] Dispersants that can be used in the production of the (meth)acrylic copolymers of the first and second aspects include, for example, surfactants that stably disperse monomers in water.Specific examples include copolymers of 2-sodium sulfoethyl methacrylate, potassium methacrylate, and methyl methacrylate, copolymers of 3-sodium sulfopropyl methacrylate, and methyl methacrylate, copolymers of sodium methacrylate and methacrylic acid, polyvinyl alcohol, polyvinylpyrrolidone, hydroxyethyl cellulose, and hydroxypropyl cellulose. These may be used alone or in combination of two or more.
[0048] Examples of dispersing aids that can be used in the production of the (meth)acrylic copolymer of the first and second embodiments include sodium sulfate, sodium carbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium chloride, calcium acetate, magnesium sulfate, and manganese sulfate. These may be used alone or in combination of two or more.
[0049] By the suspension polymerization, the (meth)acrylic copolymer of the first embodiment and the second embodiment is obtained in the form of a slurry. By dehydrating the slurry, (meth)acrylic copolymer particles usually having a shape close to a perfect sphere are obtained.
[0050] (First dehydration step, second dehydration step) The first dehydration step is a step in which the slurry after suspension polymerization is dehydrated using a dehydrator or the like to separate the (meth)acrylic copolymer particles of the first and second aspects from the reaction liquid. The second dehydration step is a step in which the (meth)acrylic copolymer particles after the washing step are dehydrated using a dehydrator or the like to separate the (meth)acrylic copolymer particles from the washing liquid.
[0051] In each dehydration step, various dehydrators can be used, for example, a centrifugal dehydrator, a device having a mechanism for sucking and removing water on a porous belt, etc. can be appropriately selected and used. One dehydrator may be used, or two of the same model may be prepared and used for each dehydration step, or multiple different models of dehydrators may be used. A model that suits the purpose can be appropriately selected from the viewpoints of product quality, capital investment cost, productivity, operating cost, etc. When the balance between product quality and production speed is important, it is preferable to use a dedicated dehydrator for each dehydration step.
[0052] (Cleaning process) The washing step is to wash the (meth)acrylic copolymer particles separated from the reaction liquid. By the washing step, components other than the (meth)acrylic copolymer are removed, and the (meth)acrylic copolymer of the first embodiment and the second embodiment is obtained. Examples of the washing method include a method in which a washing liquid is added to the (meth)acrylic copolymer particles dehydrated in the first dehydration step to re-slurry the (meth)acrylic copolymer and stir and mix it, a method in which a dehydration step is carried out in a dehydrator having a washing function, and then washing is carried out by adding a washing liquid, etc. Also, washing may be carried out by combining these washing methods.
[0053] The type and amount of the washing solution may be selected so that the purpose of the washing step is achieved. Examples of the washing solution include water (ion-exchanged water, distilled water, purified water, etc.), an aqueous solution in which a sodium salt is dissolved, a buffer adjusted to a desired pH, and methanol.
[0054] (drying process) The drying step is a step of drying the (meth)acrylic copolymer particles of the first and second aspects after the second dehydration step. Water remains on the surface of the (meth)acrylic copolymer particles after the second dehydration step. The inside of the (meth)acrylic copolymer is close to saturated water absorption. Therefore, in order to further reduce the water content of the (meth)acrylic copolymer of the first and second aspects, it is preferable to dry it.
[0055] Various types of dryers can be used for drying, including, for example, a dryer that dries by heating under reduced pressure, a dryer that uses heated air to air-transport the (meth)acrylic copolymer particles inside a pipe while drying them at the same time, and a dryer that blows heated air from below a porous plate to dry the (meth)acrylic copolymer particles above while causing them to flow. The drying step is preferably carried out so that the water content of the (meth)acrylic copolymer of the first aspect and the second aspect after the drying step is 0.01 to 10% by mass.
[0056] <Production method by bulk polymerization> The method for producing a (meth)acrylic copolymer by bulk polymerization preferably includes a bulk polymerization step and a pulverization step, and may include a devolatilization step between the bulk polymerization step and the pulverization step.
[0057] (Bulk polymerization process) The bulk polymerization step is a step of polymerizing the above-mentioned monomer (a) and monomer (b), and, if necessary, monomer (c), in the presence of a trifunctional or higher mercaptan to obtain the (meth)acrylic copolymer of the first embodiment and the second embodiment. A known method can be used for the bulk polymerization. For example, the bulk polymerization method includes a method of polymerizing the monomer (a) and the monomer (b), and optionally the monomer (c), in a reactor having a polymerization temperature control function, in the presence of a polymerization auxiliary.
[0058] Examples of the polymerization aid include a polymerization initiator, a chain transfer agent, etc. However, at least the above-mentioned trifunctional or higher mercaptan is used as the chain transfer agent. Examples of the polymerization initiator include the polymerization initiators exemplified above in the explanation of the suspension polymerization step. Examples of the chain transfer agent include the chain transfer agents exemplified above in the explanation of the suspension polymerization step.
[0059] The shape of the reactor used in the bulk polymerization process is arbitrary. For example, in a laboratory-level method, a glass cell in which a rubber tube with both ends connected to form a ring is sandwiched between two reinforced glass plates and the four corners are secured with clips can be used as the reactor. In addition, an example of an industrially used reactor is a sealed container with a stirring mechanism.
[0060] Regarding the polymerization temperature control function, for example, when the glass cell is used as the reactor, a commercially available thermostatic water bath may be used. When a sealed container having a stirring mechanism is used, the temperature can be controlled by exchanging heat with a temperature-adjusted heat medium or refrigerant from the outer surface of the reactor.
[0061] (devolatilization process) The devolatilization step is a step of removing (devolatilizing) volatile components (e.g., unreacted monomers, moisture, etc.) contained in the (meth)acrylic copolymer of the first embodiment and the second embodiment obtained in the bulk polymerization step. As the volatilization method, a known method can be used, for example, a method of treating the (meth)acrylic copolymer using a vented extruder. The set temperature of the extruder may be determined taking into consideration the boiling point of the volatile components to be removed.
[0062] (Crushing process) The pulverization step is a step in which the (meth)acrylic copolymer of the first embodiment or the second embodiment, which has been subjected to devolatilization treatment as necessary, is pulverized to a desired particle size. As the pulverization method, any pulverization method can be adopted depending on the required particle size. In order to form a slurry together with water during neutralization and dissolution in water, the maximum particle size after pulverization is preferably 5 mm or less, and more preferably 2 mm or less.
[0063] <Action and effect> The (meth)acrylic copolymers of the first and second aspects of the present invention described above have excellent solubility and powder properties, and therefore have good solubility in various solvents, particularly alkaline water. Furthermore, the compositions and inks containing the (meth)acrylic copolymers of the first and second aspects of the present invention have excellent coatability, storage stability, and hiding power in film printing, and therefore are less likely to cause bumps or uneven printing during printing. Moreover, the (meth)acrylic copolymers according to the first and second aspects of the present invention are excellent in productivity.
[0064] <Application> The (meth)acrylic copolymers according to the first and second aspects of the present invention can be used, for example, as raw materials for inks and paints, and are particularly suitable as raw materials for water-based inks.
[0065] [(Meth)acrylic copolymer composition] The (meth)acrylic copolymer composition of the present invention contains at least one selected from the group consisting of the (meth)acrylic copolymer of the first aspect and the (meth)acrylic copolymer of the second aspect of the present invention described above; water; and a basic compound. The (meth)acrylic copolymer composition may further contain a pigment and a solvent other than water (hereinafter also referred to as an "auxiliary solvent"). Hereinafter, the (meth)acrylic copolymer composition containing a pigment is also particularly referred to as a "pigment-containing composition."
[0066] The content of the (meth)acrylic copolymer is preferably 10 to 60% by mass, more preferably 15 to 50% by mass, based on the total mass of the (meth)acrylic copolymer composition. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the content of the (meth)acrylic copolymer is equal to or greater than the lower limit, the film-forming properties are good, and the texture when printed on a substrate is good. If the content of the (meth)acrylic copolymer is equal to or less than the upper limit, the film-forming properties are good, and good printing performance is exhibited on various substrates.
[0067] The water content is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total mass of the (meth)acrylic copolymer composition. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the water content is equal to or greater than the lower limit, the mixture with the pigment is good. When the water content is equal to or less than the upper limit, the viscosity after dissolving the (meth)acrylic polymer is low, and the mixture with other materials is good.
[0068] The basic compound plays the role of neutralizing the solid (meth)acrylic copolymer and dissolving it in water or a mixed solvent of water and an auxiliary solvent. Examples of the basic compound include alkali metal hydroxides, ammonia, aqueous ammonia, and amine compounds. Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the amine compound include triethylamine, 1-propylamine, diethylamine, triisopropylamine, dibutylamine, amylamine, 1-octylamine, 2-(dimethylamino)ethanol, 2-(ethylamino)ethanol, 2-(diethylamino)ethanol, 1-amino-2-propanol, 2-amino-1-propanol, 3-amino-1-propanol, 1-(dimethylamino)-2-propanol, 3-(dimethylamino)-1-propanol, 2-(propylamino)ethanol, bis(3-ethoxypropyl)amine, aminobenzyl alcohol, morpholine, N-methylmorpholine, and tetrabutylammonium hydroxide. Among these, triethylamine and 2-(dimethylamino)ethanol are preferred because they have a high amine valence per amount used, which reduces the amount of amine required for neutralization and enables the ink to have low VOCs, and they are easily volatilized after the printed matter has dried and are unlikely to remain on the printed matter. These may be used alone or in combination of two or more.
[0069] The content of the basic compound is preferably 0.1 to 10% by mass, more preferably 2 to 5% by mass, based on the total mass of the (meth)acrylic copolymer composition. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the content of the basic compound is equal to or greater than the lower limit, the solubility of the (meth)acrylic polymer composition is good. When the content of the basic compound is equal to or less than the upper limit, the water resistance after printing is good.
[0070] Examples of pigments include titanium oxide, carbon black, phthalocyanine blue, phthalocyanine green, chrome yellow, cadmium yellow, yellow lead, cobalt blue, chrome green, cobalt green, benzidine yellow, zinc white, etc. Any commercially available pigment can also be used. These may be used alone or in combination of two or more.
[0071] When the (meth)acrylic copolymer composition contains a pigment, the pigment content is preferably 20 to 60% by mass, more preferably 20 to 50% by mass, based on the total mass of the (meth)acrylic copolymer composition. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the pigment content is equal to or greater than the lower limit, the hiding power for the substrate is improved, and the color development of the coating film is good. If the pigment content is equal to or less than the upper limit, an ink in which the pigment is uniformly dispersed can be prepared, resulting in a coating film with fewer bumps.
[0072] The (meth)acrylic copolymer composition of the present invention contains water as a solvent, but may contain a solvent other than water as an auxiliary solvent, if necessary. Examples of the auxiliary solvent include water-soluble organic solvents selected from alcohols, glycols, ethers, ketones, esters, and carbitols. These may be used alone or in combination of two or more.
[0073] When the (meth)acrylic copolymer composition contains an auxiliary solvent, the content of the auxiliary solvent is preferably 1 to 40 mass %, more preferably 2 to 30 mass %, based on the total mass of the (meth)acrylic copolymer composition. The lower limit and upper limit of these numerical ranges can be arbitrarily combined. When the content of the auxiliary solvent is equal to or more than the above lower limit, the leveling property of the (meth)acrylic copolymer composition can be further improved. When the content of the auxiliary solvent is equal to or less than the above upper limit, the amount of volatile organic compounds (VOCs) contained in the (meth)acrylic copolymer composition can be reduced.
[0074] The (meth)acrylic copolymer composition can be obtained, for example, by dissolving the (meth)acrylic copolymer together with a basic compound in water or a mixed solvent of water and an auxiliary solvent. In this case, a pigment may be added as necessary. As a specific production method, a method of mixing and stirring the components constituting the (meth)acrylic copolymer composition using a commonly used stirrer can be mentioned.
[0075] The (meth)acrylic copolymer composition of the present invention described above has excellent coatability, storage stability, and hiding power in film printing, and is therefore less likely to cause bumps or uneven printing during printing.
[0076] [ink] The ink of the present invention contains the above-mentioned (meth)acrylic copolymer composition. When the (meth)acrylic copolymer composition does not contain a pigment, the ink preferably further contains a pigment in addition to the (meth)acrylic copolymer composition. When the (meth)acrylic copolymer composition is a pigment-containing composition, the pigment-containing composition itself may be used as an ink, or it may be further diluted with water or an auxiliary solvent. Furthermore, the ink may further contain auxiliary solvents, binders, and other auxiliary agents as necessary depending on various purposes.
[0077] The content of the (meth)acrylic copolymer of the first and second aspects of the present invention contained in the ink is preferably 5 to 30 mass % relative to the total mass of the ink, and more preferably 10 to 25 mass %. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the content of the (meth)acrylic copolymer is equal to or greater than the above lower limit, aggregation of primary particles of the pigment can be suppressed. If the content of the (meth)acrylic copolymer is equal to or less than the above upper limit, the ink has a low viscosity and is easy to handle.
[0078] The water content of the ink is preferably 20 to 60% by mass, and more preferably 25 to 50% by mass, based on the total mass of the ink. The lower and upper limits of these numerical ranges can be combined as desired. If the water content is equal to or greater than the lower limit, the ink will have low viscosity and be easy to print. If the water content is equal to or less than the upper limit, the ink will dry well.
[0079] The content of the basic compound contained in the ink is preferably 0.1 to 10% by mass, more preferably 2 to 5% by mass, based on the total mass of the ink. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the content of the basic compound is equal to or greater than the lower limit, the ink has good film-forming properties. When the content of the basic compound is equal to or less than the upper limit, an image with good water resistance can be formed.
[0080] Examples of the pigment include the pigments exemplified above in the description of the (meth)acrylic copolymer composition. The content of the pigment contained in the ink is preferably 10 to 50% by mass, more preferably 20 to 40% by mass, based on the total mass of the ink. The lower and upper limits of these numerical ranges can be arbitrarily combined. If the content of the pigment is equal to or greater than the lower limit, the ink will have excellent hiding power for the substrate. If the content of the pigment is equal to or less than the upper limit, the generation of aggregates during printing is suppressed, resulting in an ink with less color unevenness.
[0081] The ink of the present invention contains water as a solvent, but may contain a solvent other than water as an auxiliary solvent, if necessary. Examples of the auxiliary solvent include the auxiliary solvents exemplified above in the explanation of the (meth)acrylic copolymer composition. When the ink contains an auxiliary solvent, the content of the auxiliary solvent is preferably 0.1 to 30 mass % relative to the total mass of the ink, and more preferably 1 to 25 mass %. The lower and upper limits of these numerical ranges can be arbitrarily combined. When the content of the auxiliary solvent is equal to or greater than the above lower limit, the leveling properties of the water-based ink can be further improved. When the content of the auxiliary solvent is equal to or less than the above upper limit, the amount of volatile organic compounds (VOCs) contained in the ink can be reduced.
[0082] The ink of the present invention may contain a binder for the purpose of improving the adhesion of the ink to the substrate. Examples of the binder include urethane dispersions (PUD), urethane-acrylic composite dispersions (PUA), acrylic emulsions, polyester dispersions, polyolefin dispersions, polyolefin-acrylic composite dispersions, and polyolefin-polyester dispersions. These may be used alone or in combination of two or more.
[0083] Examples of other auxiliary agents include a defoaming agent, a leveling agent, a pigment dispersant, a film-forming auxiliary, and an adhesion promoter. These may be used alone or in combination of two or more.
[0084] The ink can be obtained, for example, by adding a pigment and, if necessary, one or more of a cosolvent, a binder, and other auxiliaries to a (meth)acrylic copolymer composition and mixing them. At this time, if necessary, a pigment dispersion treatment may be performed. In addition, if necessary, the ink may be further diluted with water. As a method for dispersing the pigment, any dispersion treatment method can be adopted, such as a commercially available rocking shaker, planetary bead mill, batch type stirring bead mill, or continuous stirring bead mill.
[0085] The ink of the present invention described above has excellent coatability, storage stability, and hiding power in film printing, and is therefore less likely to cause bumps or uneven printing during printing. EXAMPLES
[0086] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. The various measurement and evaluation methods in the following examples and comparative examples are as follows. In the following description, unless otherwise specified, "parts" means parts by mass and "%" means % by mass.
[0087] [Measurement and evaluation method] <Measurement of second order glass transition temperature (Tg)> Using a differential scanning calorimeter (Seiko Instruments Inc., "EXSTAR DSC-6200"), 5 mg of the (meth)acrylic copolymer was subjected to a temperature increase / decrease operation under the following temperature scanning conditions. The DSC data measured in step (3) under the following temperature scanning conditions was plotted with temperature (°C) on the horizontal axis and DSC measurement value (mW) on the vertical axis. The temperature (°C) corresponding to the intersection of a tangent drawn to a point on the low temperature side among the points where the rate of change of the slope of the graph is 0 and a tangent to a point (inflection point) where the rate of change of the slope of the graph is maximum was determined as the second order glass transition temperature (Tg) of the (meth)acrylic copolymer. (Temperature scanning conditions) Step (1): After stabilizing at -10℃ for 5 minutes, heat to 110℃. Step (2): Cool to -10°C. Step (3): Heat again to 110°C. Step (4): Cool to room temperature. Heating rate: +10℃ / min. ·Cooling rate: -10℃ / min.
[0088] <Acid value measurement> Approximately 0.5 g of (meth)acrylic copolymer was precisely weighed into a beaker (A(g)), and 50 mL of a mixed solution of toluene and ethanol (mass ratio 1:1) was added. A few drops of phenolphthalein were added, and titration was performed with 0.05N KOH solution (solvent: ethanol). (Titer amount = B(mL), titer of KOH solution = f). A blank measurement was also performed in the same manner (titer amount = C(mL)), and calculation was performed according to the following formula. Acid value (mgKOH / g)={(BC)×0.05×56.11×f} / A
[0089] <Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn)> The weight average molecular weight (Mw) and number average molecular weight (Mn) of the (meth)acrylic copolymer were measured by gel permeation chromatography (GPC) and calculated as polystyrene equivalent values using a calibration curve of standard polystyrene. The GPC measurement conditions were as follows. (GPC measurement conditions) - Equipment: "HLC-8220GPC" manufactured by Tosoh Corporation. Column: Tosoh Corporation's "TSKgel G5000HXL (7.8mmφ×300mm)" and "GMHXL-L (7.8mmφ×300mm)" connected in series. Eluent: Tetrahydrofuran. Sample concentration: 0.4%. ·Measurement temperature: 40℃. ·Injection volume: 100μL. ·Flow rate: 1.0mL / min. Detectors: RI (built into the device), UV (Tosoh UV-8220).
[0090] <Moisture content measurement> The moisture content of the (meth)acrylic copolymer was calculated from the loss on drying of the (meth)acrylic copolymer before and after drying at 105°C for 2 hours, assuming that the moisture content when the (meth)acrylic copolymer was dried at 105°C for 2 hours was 0%.
[0091] <Evaluation of solubility in alkaline water> 65.5 g of water and 30.0 g of a (meth)acrylic copolymer were placed in a glass bottle ("M-225" manufactured by Kashiwa Glass Co., Ltd.) together with a stirrer, the bottle was closed, and the bottle was stirred for 10 minutes in a water bath adjusted to 30°C to form a slurry. 4.5 g of 2-(dimethylamino)ethanol was added to the resulting slurry, and the solution was visually inspected for solubility after stirring for an additional 3 hours at 30°C. If a precipitate was present in the solution, the solution was stirred for an additional 3 hours, and the solubility in alkaline water was evaluated according to the following evaluation criteria. A: After the first 3 hours of stirring, no precipitate was visible and the solubility was excellent. A-: After the first 3 hours of stirring, a precipitate was visually observed, but after an additional 3 hours of stirring, the precipitate disappeared, indicating excellent solubility. B: Even after stirring for 6 hours, insoluble matter was clearly precipitated, and the solubility was poor.
[0092] <Evaluation of storage stability and hiding power> (Preparation of (Meth)Acrylic Copolymer Composition) 65.5 g of water and 30.0 g of the (meth)acrylic copolymer were placed in a glass bottle ("M-225" manufactured by Kashiwa Glass Co., Ltd.) together with a stirrer, the bottle was closed, and the bottle was stirred at room temperature for 10 minutes to obtain a slurry. 4.5 g of 2-(dimethylamino)ethanol was added to the obtained slurry, which was then placed in a water bath at 60°C and stirred until no undissolved material remained, to obtain a (meth)acrylic copolymer composition having a concentration of 30% (meth)acrylic copolymer.
[0093] (Ink Preparation) 50 g of the obtained (meth)acrylic copolymer composition, 30 g of titanium oxide CR-90 (manufactured by Ishihara Sangyo Kaisha, Ltd.), 20 g of 2-propanol, and 60 g of glass beads were mixed in a container, and then dispersed for 1 hour using a rocking shaker. The glass beads were then removed from the obtained mixture to obtain a pigment paste. 60 g of the resulting pigment paste was diluted with 11 g of 2-propanol and 13 g of water to obtain a water-based ink. The resulting water-based ink was used to evaluate the storage stability of the ink and the hiding power of the printed matter.
[0094] (Evaluation of storage stability) The ink was allowed to stand at room temperature for 3 days, and the presence or absence of pigment sedimentation was visually confirmed, and the storage stability was evaluated according to the following evaluation criteria. A: The pigment remains dispersed in the ink even after three days. B: After 3 days, some or all of the pigment in the ink has settled.
[0095] (Evaluation of concealment) The ink was set in a gravure printing machine (RK PRINTCOAT INSTRUMENTS, "GP-100") and printing was performed. A printing plate with 150 lines / inch was used. A propylene film (Toyobo Co., Ltd., "Pylen (registered trademark) Film OT P2108") was used as the substrate to be printed. The color difference of the transmitted light was measured for the coating film after printing using a spectrophotometer (Konica Minolta, Inc., "CM-5"). * The ΔL value was calculated by subtracting 100 from the measured value (brightness), and the hiding power was evaluated according to the following criteria. The smaller the ΔL value, the better the hiding power of the print. A: △L value ≦-22.5. B: △L value > -22.5.
[0096] [Production of Dispersant (1)] In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 1230 g of deionized water, 60 g of sodium 2-sulfoethyl methacrylate, 10 g of potassium methacrylate, and 12 g of methyl methacrylate were added and stirred, and the polymerization temperature was raised to 50°C while replacing the atmosphere in the polymerization apparatus with nitrogen, and 0.08 g of 2,2'-azobis(2-methylpropionamidine) dihydrochloride was added as a polymerization initiator, and the polymerization temperature was further raised to 60°C. Simultaneously with the addition of the polymerization initiator, methyl methacrylate was continuously dropped at a rate of 0.24 g / min using a dropping pump for 75 minutes, and the polymerization temperature was maintained at 60°C for 6 hours, and then cooled to room temperature to obtain dispersant (1). The solid content of the obtained dispersant (1) was 7.5%.
[0097] [Example 1] In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, a monomer mixture in which 40 parts of methyl methacrylate, 40 parts of n-butyl methacrylate, 5 parts of n-butyl acrylate, 15 parts of methacrylic acid, and 1.2 parts of trimethylolpropane trimethacrylate were uniformly dissolved, and 0.4 parts of 2,2'-azobis(2-methylbutyronitrile), 2 parts of 2-ethylhexyl 3-mercaptopropionate, 2 parts of trimethylolpropane tris(3-mercaptopropionate), and 2 parts of pentaerythritol tetrakis(thioglycolate) were added and stirred until uniform. Furthermore, a mixture of 160 parts of pure water, 0.1 parts of sodium sulfate, and 0.6 parts of dispersant (1) was added, and nitrogen substitution was performed while stirring. Thereafter, the temperature inside the flask was controlled at 80° C. to initiate suspension polymerization, and after the peak of the polymerization heat was detected, the mixture was treated at 90° C. for 30 minutes to obtain a (meth)acrylic copolymer slurry (suspension polymerization step). After the polymerization, the inside of the vessel was cooled to room temperature, and the resulting slurry was dehydrated by a centrifugal dehydrator (first dehydration step). The obtained (meth)acrylic copolymer and pure water as a washing solution were charged into a washing tank so that the mass ratio ((meth)acrylic copolymer: washing solution) was 1:2, and the mixture was stirred and mixed for 20 minutes to wash (washing step), and then dehydrated using a centrifugal dehydrator (second dehydration step). After dehydration, the dehydrated (meth)acrylic copolymer was placed in a fluidized-bed dryer with an internal temperature set at 40°C, and dried until the moisture content of the (meth)acrylic copolymer particles became 10% or less (drying step). The second order glass transition temperature (Tg), acid value, weight average molecular weight (Mw) and number average molecular weight (Mn) of the obtained particulate solid (meth)acrylic copolymer particles were measured, and the solubility in alkaline water was evaluated. In addition, a water-based ink was prepared by the above-mentioned method, and the storage stability of the ink and the hiding power of the printed matter were evaluated. The results are shown in Table 1.
[0098] [Examples 2, 3, 5, 6, Comparative Examples 1 to 7] Particulate solid (meth)acrylic copolymer particles were produced in the same manner as in Example 1, except for using the blending compositions shown in Tables 1 and 2, and various measurements and evaluations were carried out. The results are shown in Table 1.
[0099] [Example 4] A homogeneous mixture of 70 parts of methyl methacrylate, 5 parts of n-butyl acrylate, 12 parts of 2-ethylhexyl acrylate, 13 parts of methacrylic acid, 1.2 parts of trimethylolpropane triacrylate, 0.4 parts of tert-butyl peroxy-2-ethylhexanoate (manufactured by NOF Corporation, "Perbutyl O"), 4 parts of 2-ethylhexyl 3-mercaptopropionate, and 2 parts of pentaerythritol tetrakis(thioglycolate) was placed in a glass cell equipped with a thermometer and sealed, and then bulk polymerization was initiated by controlling the temperature inside the glass cell to 83°C in a water bath. After the peak of the heat generated by polymerization was detected, the mixture was treated at 90°C for 30 minutes to obtain a bulk solid (meth)acrylic copolymer (bulk polymerization process). After polymerization, the inside of the glass cell was cooled to room temperature. The solid (meth)acrylic copolymer in the form of a lump was removed from the cell and crushed with a Sanitary Crusher SC-01 (manufactured by Sansho Industry Co., Ltd.), then shaken on a mesh with 2 mm openings, and the part that passed through was collected to obtain a particulate solid (meth)acrylic copolymer (crushing step). The second order glass transition temperature (Tg), acid value, weight average molecular weight (Mw) and number average molecular weight (Mn) of the obtained particulate solid (meth)acrylic copolymer were measured, and the solubility in alkaline water was evaluated. In addition, a water-based ink was prepared by the above-mentioned method, and the storage stability of the ink and the hiding power of the printed matter were evaluated. The results are shown in Table 1.
[0100] [Example 5] The particulate solid (meth)acrylic copolymer obtained in Example 4 was shaken on a mesh with 1 mm openings for 5 minutes, and the part that passed through was collected to obtain a particulate solid (meth)acrylic copolymer.
[0101] [Example 6] The particulate (meth)acrylic copolymer obtained in Example 4 was shaken on a mesh having an opening of 750 μm for 5 minutes, and the part that passed through was collected to obtain a particulate solid (meth)acrylic copolymer.
[0102] [Table 1]
[0103] [Table 2]
[0104] The abbreviations in the table are as follows: Furthermore, blank spaces in the table mean that the component was not blended (0 parts blended). · MMA: Methyl methacrylate. · n-BMA: n-Butyl methacrylate. · n-BA: n-Butyl acrylate. · 2-EHA: 2-Ethylhexyl acrylate. ·IBXMA: Isobornyl methacrylate. · MAA: Methacrylic acid. · TMPTMA: Trimethylolpropane trimethacrylate. · HDDA: 1,6-Hexanediol diacrylate. · TMPTA: Trimethylolpropane triacrylate. · EHMP: 2-ethylhexyl 3-mercaptopropionate. · EGMP: Ethylene glycol bis(3-mercaptopropionate). · TMPMP: Trimethylolpropane tris(3-mercaptopropionate). ·PEMP: Pentaerythritol tetrakis(3-mercaptopropionate). ·PETG: Pentaerythritol tetrakis(thioglycolate). ·AMBN: 2,2'-Azobis(2-methylbutyronitrile). · Perbutyl O: tert-butyl peroxy-2-ethylhexanoate. IBXMA is a substitute for monomer (a) (monomer (a')).
[0105] As is clear from the results in Table 1, the (meth)acrylic copolymers obtained in each Example had good solubility in alkaline water. In addition, the inks containing these (meth)acrylic copolymers had good storage stability and were excellent in the concealment of printed matter when printed on film.
[0106] On the other hand, as is clear from the results in Table 2, in the case of Comparative Examples 1 and 2 in which a (meth)acrylic copolymer having a chemical structure derived from a monofunctional mercaptan instead of a chemical structure derived from a trifunctional or higher functional mercaptan was used, the storage stability of the ink and the hiding power of the printed matter were poor. The (meth)acrylic copolymer of Comparative Example 3, which does not have a chemical structure derived from a trifunctional or higher functional mercaptan but has a chemical structure derived from a monofunctional mercaptan instead and has a structural unit derived from HDDA (1,6-hexanediol diacrylate) as a structural unit derived from monomer (c2), had poor solubility in alkaline water. In addition, in the case of Comparative Example 3, although a (meth)acrylic copolymer composition was obtained, the viscosity was very high and it was not possible to carry out a dispersion treatment of the pigment, so that it was not possible to evaluate the storage stability of the ink and the hiding power of the printed matter. The (meth)acrylic copolymers of Comparative Examples 4 and 5, which do not have a chemical structure derived from a trifunctional or higher functional mercaptan, but instead have a chemical structure derived from a monofunctional mercaptan or a chemical structure derived from a bifunctional mercaptan, but the proportion of the structure is smaller than that of Comparative Examples 1 and 2, did not dissolve in the eluent and could not be subjected to GPC measurement. In addition, the solubility in alkaline water was poor. Furthermore, in the cases of Comparative Examples 4 and 5, although a (meth)acrylic copolymer composition was obtained, the viscosity was very high and it was not possible to perform a pigment dispersion treatment, so that it was not possible to evaluate the storage stability of the ink and the hiding power of the printed matter. The (meth)acrylic copolymers of Comparative Examples 6 and 7, which did not have a constituent unit derived from monomer (a) or a constituent unit derived from monomer (b), had poor solubility in alkaline water. In addition, in the case of Comparative Examples 6 and 7, the (meth)acrylic copolymer was not completely dissolved in alkaline water, and it was not possible to prepare a (meth)acrylic copolymer composition and ink, so that it was not possible to evaluate the storage stability of the ink and the hiding power of the printed matter. [Industrial Applicability]
[0107] According to the present invention, it is possible to provide a (meth)acrylic copolymer having good solubility in alkaline water, and having good storage stability of ink and good hiding power in film printing, a (meth)acrylic copolymer composition containing the (meth)acrylic copolymer, and an ink containing the (meth)acrylic copolymer composition. Therefore, the (meth)acrylic copolymer of the present invention can be suitably used in the field of resin compositions that can be developed with an alkaline aqueous solution, and is extremely important industrially.
Claims
1. The present invention relates to a particulate solid having a structural unit derived from an alkyl (meth)acrylate ester having an alkyl group with 1 to 8 carbon atoms, a structural unit derived from an acid group-containing vinyl compound, and a chemical structure derived from a tri- or higher functional mercaptan, A (meth)acrylic copolymer having a second-order glass transition temperature of 35° C. or higher and 67° C. or lower.
2. a structural unit derived from a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, a structural unit derived from an acid group-containing vinyl compound, and a chemical structure derived from a tri- or higher functional mercaptan, and further having one or more chemical structures selected from the group consisting of a chemical structure derived from a monofunctional mercaptan and a chemical structure derived from a difunctional mercaptan, A (meth)acrylic copolymer having a second-order glass transition temperature of 35° C. or higher and 67° C. or lower.
3. The (meth)acrylic copolymer described in claim 2, wherein the (meth)acrylic copolymer is a particulate solid.
4. The (meth)acrylic copolymer according to claim 1 or 3, further comprising a structural unit derived from a compound having two or more polymerizable double bonds.
5. The (meth)acrylic copolymer according to claim 1 or 4, further comprising at least one chemical structure selected from the group consisting of a chemical structure derived from a monofunctional mercaptan and a chemical structure derived from a difunctional mercaptan.
6. The (meth)acrylic copolymer according to any one of claims 1, 3, 4 and 5, wherein the (meth)acrylic copolymer has a mass average particle size of 20 to 2000 µm.
7. The (meth)acrylic copolymer according to any one of claims 1 to 6, wherein the (meth)acrylic copolymer has a water content of 0.01 to 10 mass%.
8. The (meth)acrylic copolymer according to any one of claims 1 to 7, wherein the (meth)acrylic copolymer has an acid value of 20 to 140 mg KOH / g.
9. The (meth)acrylic copolymer according to any one of claims 1 to 8, wherein the (meth)acrylic copolymer has a weight average molecular weight of 15,000 to 80,000.
10. A (meth)acrylic copolymer composition comprising the (meth)acrylic copolymer according to any one of claims 1 to 9, water, and a basic compound.
11. The (meth)acrylic copolymer composition according to claim 10 , further comprising a pigment.
12. An ink comprising the (meth)acrylic copolymer composition according to claim 10 or 11.
Citation Information
Patent Citations
Synthetic resin for preparation of protective coatings and process for preparation of coatings on the basis of such resin
EP3587459A1
Coating material binder that is based on acrylic ester copolymer and can be diluted with water
JP1992304277A
UV ray-curable hot-melt adhesive composition
JP2005097406A
Reactive hot melt composition for automobile lamp tool and automobile lamp fitting
JP2016196626A
Ink, ink set, inkjet recording method, and manufacturing method of ink
JP2019163417A