Negative-type photosensitive resin composition, and method for producing polyimide and cured relief pattern using the same
The combination of a polyimide precursor, (meth)acrylate, and photopolymerization initiator in a negative photosensitive resin composition addresses void formation and adhesion issues, enhancing chemical resistance and resolution for semiconductor devices, particularly in flip-chip mounting applications.
Patent Information
- Application Number
- JP2022184276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-26
- Filing Date
- 2022-11-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-07-18
AI Technical Summary
Conventional photosensitive resin compositions used in semiconductor devices face issues with void formation at the interface of the Cu layer and resin layer during high-temperature storage tests, leading to deteriorated adhesion and insufficient chemical resistance, which is exacerbated by the demands for miniaturization and precise wiring control in high-end applications like flip-chip mounting.
A negative photosensitive resin composition is developed, combining a polyimide precursor with specific structures, a (meth)acrylate compound, and a photopolymerization initiator, along with optional additives like urethane/urea compounds and silane coupling agents, to enhance adhesion and chemical resistance, thereby reducing void formation and improving resolution.
The composition effectively suppresses voids at the Cu-resin interface after high-temperature storage tests, ensuring high adhesion to mold resins in fan-out type semiconductor packages and maintaining chemical resistance, thus supporting precise wiring and miniaturization requirements.
Smart Images

Figure 0007590394000001 
Figure 0007590394000002 
Figure 0007590394000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative-type photosensitive resin composition, and a method for producing a polyimide and a cured relief pattern using the same. [Background technology]
[0002] Conventionally, polyimide resins, polybenzoxazole resins, phenolic resins, etc., which have excellent heat resistance, electrical properties, and mechanical properties, have been used as insulating materials for electronic components, and passivation films, surface protective films, interlayer insulating films, etc. for semiconductor devices. Among these resins, those provided in the form of a photosensitive resin composition can easily form a heat-resistant relief pattern film by applying, exposing, developing, and curing the composition to a thermal imidization treatment. Such photosensitive resin compositions have the characteristic of enabling a significant reduction in the process compared to conventional non-photosensitive materials.
[0003] Incidentally, semiconductor devices (hereinafter also referred to as "elements") are mounted on printed circuit boards by various methods according to the purpose. Conventional elements were generally fabricated by a wire bonding method in which thin wires connect the external terminals (pads) of the element to a lead frame. However, in recent years, elements have become faster and the operating frequency has reached GHz, so that differences in the wiring length of each terminal during mounting have begun to affect the operation of the element. As a result, when mounting elements for high-end applications, it has become necessary to accurately control the length of the mounting wiring, and it has become difficult to meet this requirement using wire bonding.
[0004] Therefore, flip-chip mounting has been proposed, in which a rewiring layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed thereon, and then the chip is flipped over and directly mounted on a printed circuit board (see, for example, Patent Document 1). This flip-chip mounting allows accurate control of wiring distance, and is therefore adopted for high-end devices that handle high-speed signals, and for mobile phones and the like due to its small mounting size, and demand is rapidly expanding. When materials such as polyimide, polybenzoxazole, and phenolic resin are used for flip-chip mounting, a metal wiring layer formation process is performed after the resin layer pattern is formed. The metal wiring layer is usually formed by roughening the surface of the resin layer by plasma etching, forming a metal layer to be a plating seed layer by sputtering to a thickness of 1 μm or less, and performing electrolytic plating using the metal layer as an electrode. In this case, titanium (Ti) is generally used as the metal that becomes the seed layer, and copper (Cu) is generally used as the metal for the rewiring layer formed by electrolytic plating.
[0005] For such a metal rewiring layer, it is required that the rewired metal layer and the resin layer have high adhesion after a reliability test. Examples of the reliability test include a high-temperature storage test in which the device is stored in air at a high temperature of 125°C or higher for 100 hours or more; a high-temperature operation test in which the device is stored in air at a temperature of about 125°C for 100 hours or more while wiring is assembled and a voltage is applied; a temperature cycle test in which the device is cycled between a low-temperature state of about -65°C to -40°C and a high-temperature state of about 125°C to 150°C in air; a high-temperature and high-humidity storage test in which the device is stored in a water vapor atmosphere at a temperature of 85°C or higher and a humidity of 85% or higher; a high-temperature and high-humidity bias test in which the same test as the high-temperature and high-humidity storage test is performed while wiring is assembled and a voltage is applied; and a solder reflow test in which the device is passed through a solder reflow furnace at 260°C multiple times in air or under nitrogen. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-338947 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the past, in the case of a high-temperature storage test among the above reliability tests, there was a problem that voids were generated at the interface between the rewired Cu layer and the resin layer after the test. When voids are generated at the interface between the Cu layer and the resin layer, the adhesion between the two layers decreases.
[0008] In addition to the problem of voids, the metal redistribution layer is required to have chemical resistance, and the demand for finer patterning is also increasing. For this reason, photosensitive resin compositions used in particular for forming the redistribution layer of semiconductors are required to suppress the generation of voids and to exhibit high chemical resistance and resolution.
[0009] The present invention has been devised in view of such conventional circumstances, and has as its object to provide a negative-type photosensitive resin composition (hereinafter, also simply referred to as "photosensitive resin composition" in the present specification) that can provide high chemical resistance and resolution and can suppress the generation of voids at the interface where the Cu layer contacts the resin layer after a high temperature storage test. Another object is to provide a method for forming a cured relief pattern using the negative-type photosensitive resin composition of the present invention.
[0010] In addition, fan-out type semiconductor packages have been attracting attention in recent years. In fan-out type semiconductor packages, a chip sealing body larger than the chip size of the semiconductor chip is formed by covering the semiconductor chip with an encapsulant. Furthermore, a redistribution layer is formed that extends to the area of the semiconductor chip and the encapsulant. The redistribution layer is formed with a thin film thickness. Furthermore, since the redistribution layer can be formed up to the area of the encapsulant, the number of external connection terminals can be increased. Fan-out type semiconductor packages require a further reduction in the curing temperature, which results in a decrease in adhesion with encapsulants such as mold resin, and therefore further improvements are required. [Means for solving the problem]
[0011] The present inventors have found that the above problems can be solved by combining a polyimide precursor having a specific structure, a (meth)acrylate having a specific structure, and a photopolymerization initiator, and have completed the present invention. Examples of embodiments of the present invention are listed below. [1] (A) a polyimide precursor represented by the following general formula (1): (B) a compound containing at least one selected from a urethane bond and a urea bond; and (C) Photopolymerization initiator A negative type photosensitive resin composition comprising: [ka] In the formula, X1 is a tetravalent organic group, Y1 is a divalent organic group, n1 is an integer from 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group, and at least one of R1 and R2 is a monovalent organic group represented by the following general formula (2). [ka] {In the formula, L1, L2, and L3 each independently represent a hydrogen atom or an organic group having 1 to 3 carbon atoms, and m1 represents an integer of 2 to 10.} [2] 2. The negative photosensitive resin composition according to item 1, wherein the compound (B) is a compound having a urea bond. [3] 3. The negative type photosensitive resin composition according to item 1 or 2, wherein the compound (B) further contains at least one functional group selected from a (meth)acrylic group, a hydroxyl group, an alkoxy group, and an amino group. [4] The negative type photosensitive resin composition according to any one of items 1 to 3, wherein the compound (B) is a compound having a (meth)acrylic group and a urea bond and has a (meth)acrylic equivalent of 150 to 400 g / mol. [5] The negative type photosensitive resin composition according to any one of items 1 to 3, wherein the compound (B) is a compound having a (meth)acrylic group and a urea bond and has a (meth)acrylic equivalent of 210 to 400 g / mol. [6] The negative type photosensitive resin composition according to any one of items 1 to 3, wherein the compound (B) is a compound having a (meth)acrylic group and a urea bond and has a (meth)acrylic equivalent of 220 to 400 g / mol. [7] 7. The negative photosensitive resin composition according to any one of items 1 to 6, wherein the compound (B) has a structure represented by the following general formula (3): [ka] {In the formula, R3 is a hydrogen atom or a methyl group, A is a group selected from the group consisting of -O-, -NH-, and -NL4-, L4 is a monovalent organic group having 1 to 12 carbon atoms, Z1 is an m2-valent organic group having 2 to 24 carbon atoms, Z2 is a divalent organic group having 2 to 8 carbon atoms, and m2 is an integer of 1 to 3.} [8] The negative type photosensitive resin composition according to any one of items 1 to 7, wherein the compound (B) further contains a (meth)acrylic group and at least one functional group selected from a hydroxyl group, an alkoxy group, and an amino group. [9] The negative type photosensitive resin composition according to any one of items 1 to 8, wherein the compound (B) is at least one compound selected from the group consisting of the following formulas (4) to (7) and (11) to (14): [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[10] 10. The negative type photosensitive resin composition according to any one of items 1 to 9, further comprising (D) a rust inhibitor.
[11] 11. The negative type photosensitive resin composition according to item 10, wherein the (D) rust inhibitor contains a nitrogen-containing heterocyclic compound.
[12] Item 12. The negative type photosensitive resin composition according to item 11, wherein the nitrogen-containing heterocyclic compound is an azole compound.
[13] Item 12. The negative type photosensitive resin composition according to item 11, wherein the nitrogen-containing heterocyclic compound is a purine derivative.
[14] 14. The negative type photosensitive resin composition according to any one of items 1 to 13, further comprising (E) a silane coupling agent.
[15] 15. The negative type photosensitive resin composition according to any one of items 1 to 14, wherein X1 in the polyimide precursor (A) includes at least one selected from the group consisting of the following general formulae (20a), (20b) and (20c): [ka] [ka] [ka] In the formula, R6 is independently a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 where l is an integer selected from 0 to 2, and m is an integer selected from 0 to 3.}
[16] 16. The negative type photosensitive resin composition according to any one of items 1 to 15, wherein Y1 in the polyimide precursor (A) includes at least one selected from the group consisting of the following general formulae (21a), (21b) and (21c): [ka] [ka] [ka] In the formula, R6 is independently a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 and n is an integer selected from 0 to 4.}
[17] The polyimide precursor (A) is represented by the following general formula (8): [ka] {In the formula, n1 is an integer of 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group.} 17. The negative type photosensitive resin composition according to any one of items 1 to 16, comprising a polyimide precursor having a structural unit represented by the following formula:
[18] The polyimide precursor (A) is represented by the following general formula (9): [ka] {In the formula, n1 is an integer of 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group.} 18. The negative type photosensitive resin composition according to any one of items 1 to 17, comprising a polyimide precursor having a structural unit represented by the following formula:
[19] The polyimide precursor (A) is represented by the following general formula (8): [ka] {In the formula, n1 is an integer of 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group, and may be the same as or different from R1, R2, and n1 in general formula (9).} A structural unit represented by The following general formula (9): [ka] {In the formula, n1 is an integer of 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group, and may be the same as or different from R1, R2, and n1 in general formula (8).} or a copolymer with a structural unit represented by 19. The negative type photosensitive resin composition according to any one of items 1 to 18, which is a blend of a polyimide precursor having a structural unit represented by the general formula (8) and a polyimide precursor having a structural unit represented by the general formula (9).
[20] Item 20. The negative photosensitive resin composition according to item 19, wherein the polyimide precursor (A) is a copolymer of a structural unit represented by the general formula (8) and a structural unit represented by the general formula (9). [twenty one] 100 parts by mass of the polyimide precursor (A); 0.1 to 30 parts by mass of the (B) compound based on 100 parts by mass of the (A) polyimide precursor; 0.1 to 20 parts by mass of the photopolymerization initiator (C) based on 100 parts by mass of the polyimide precursor (A); 21. The negative type photosensitive resin composition according to any one of items 1 to 20, comprising: [twenty two] 22. A method for producing a polyimide, comprising a step of converting the negative type photosensitive resin composition according to any one of items 1 to 21 into a polyimide. [twenty three] (1) A step of applying the negative type photosensitive resin composition according to any one of items 1 to 21 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat-treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising: [twenty four] A compound represented by the following formula (5): [ka] [twenty five] A compound represented by the following formula (6): [ka]
[26] A compound represented by the following formula (7): [ka]
[27] A compound represented by the following formula (11): [ka]
[28] A compound represented by the following formula (12): [ka]
[29] A compound represented by the following formula (13): [ka]
[30] A compound represented by the following formula (14): [ka] Effect of the Invention
[0012] According to the present invention, it is possible to provide a negative-type photosensitive resin composition that has high chemical resistance and resolution and suppresses the generation of voids at the interface of the Cu layer and the resin layer after a high temperature storage test, and also to provide a method for forming a cured relief pattern using the negative-type photosensitive resin composition. Also, according to the present invention, it is possible to provide a negative-type photosensitive resin composition that has good adhesion to a mold resin used in a fan-out type semiconductor package. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiment for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out with various modifications within the scope of the gist. Note that throughout this specification, structures represented by the same symbol in a general formula may be the same or different when multiple structures are present in a molecule.
[0014] <Negative-type photosensitive resin composition> The negative type photosensitive resin composition according to this embodiment contains (A) a polyimide precursor; (B) a compound containing at least one selected from a urethane bond and a urea bond; and (C) a photopolymerization initiator.
[0015] From the viewpoint of obtaining high chemical resistance, the negative type photosensitive resin composition preferably contains 100 parts by mass of (A) polyimide precursor, 0.1 to 30 parts by mass of (B) compound based on 100 parts by mass of (A) polyimide precursor, and 0.1 to 20 parts by mass of (C) photopolymerization initiator based on 100 parts by mass of (A) polyimide precursor.
[0016] (A) Polyimide precursor The polyimide precursor (A) in this embodiment is a resin component contained in a negative photosensitive resin composition, and is converted to a polyimide by a thermal cyclization treatment. The polyimide precursor is a polyamide having a structure represented by the following general formula (1). [ka] In the formula, X1 is a tetravalent organic group, Y1 is a divalent organic group, n1 is an integer from 2 to 150, and R1 and R2 are each independently a hydrogen atom or a monovalent organic group.
[0017] At least one of R1 and R2 is a monovalent organic group represented by the following general formula (2). [ka] {In the formula, L1, L2, and L3 each independently represent a hydrogen atom or an organic group having 1 to 3 carbon atoms, and m1 represents an integer of 2 to 10.}
[0018] In the general formula (1), n1 is not limited as long as it is an integer of 2 to 150, but from the viewpoint of the photosensitive properties and mechanical properties of the negative photosensitive resin composition, an integer of 3 to 100 is preferable, and an integer of 5 to 70 is more preferable. In the general formula (1), the tetravalent organic group represented by X1 is preferably an organic group having 6 to 40 carbon atoms, more preferably an aromatic group in which -COOR1 group, -COOR2 group and -CONH- group are in the ortho position with respect to each other, or an alicyclic aliphatic group, in order to achieve both heat resistance and photosensitive properties. Specific examples of the tetravalent organic group represented by X1 include organic groups having 6 to 40 carbon atoms containing an aromatic ring, such as a group having a structure represented by the following general formula (20), but are not limited thereto. [ka] In the formula, R6 is a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 where l is an integer selected from 0 to 2, m is an integer selected from 0 to 3, and n is an integer selected from 0 to 4.}
[0019] The structure of X1 may be one type or a combination of two or more types. The X1 group having the structure represented by the above formula (20) is particularly preferred in terms of achieving both heat resistance and photosensitive properties. As the X1 group, among the structures represented by the above formula (20), the structures represented by the following formulas (20a), (20b) and (20c) are particularly preferred in terms of chemical resistance, resolution and void suppression after high-temperature storage test. [ka] In the formula, R6 is independently a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 where l is an integer selected from 0 to 2, m is an integer selected from 0 to 3, and n is an integer selected from 0 to 4.}R6 in general formulae (20a) to (20c) may be the same as or different from R6 in general formulae (21a) to (21c) described below.
[0020] In the above general formula (1), the divalent organic group represented by Y1 is preferably an aromatic group having 6 to 40 carbon atoms in order to achieve both heat resistance and photosensitive properties, and examples thereof include, but are not limited to, structures represented by the following formula (21). [ka] In the formula, R6 is a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 and n is an integer selected from 0 to 4.}
[0021] The structure of Y1 may be one type or a combination of two or more types. The Y1 group having the structure represented by the above formula (21) is particularly preferred in terms of achieving both heat resistance and photosensitive properties. As the Y1 group, among the structures represented by the above formula (21), the structures represented by the following formulas (21a), (21b) and (21c) are particularly preferred in terms of chemical resistance, resolution and void suppression after high-temperature storage test. [ka] In the formula, R6 is independently a hydrogen atom, a fluorine atom, or a C 10 Hydrocarbon groups of C1 to C 10 and n is an integer selected from 0 to 4.}R6 in general formulae (21a) to (21c) may be the same as or different from R6 in general formulae (20a) to (20c) described above.
[0022] In the above general formula (2), L1 is preferably a hydrogen atom or a methyl group, and L2 and L3 are preferably hydrogen atoms from the viewpoint of photosensitive properties. Also, m1 is an integer of 2 to 10, preferably an integer of 2 to 4, from the viewpoint of photosensitive properties.
[0023] In one embodiment, the polyimide precursor (A) is represented by the following general formula (8): [ka] {wherein R1, R2, and n1 are defined above.} In the general formula (8), at least one of R1 and R2 is more preferably a monovalent organic group represented by the above general formula (2). When the (A) polyimide precursor contains a polyimide precursor having a structural unit represented by the general formula (8), the effect of the resolution is particularly enhanced.
[0024] In one embodiment, the polyimide precursor (A) is represented by the following general formula (9): [ka] {wherein R1, R2, and n1 are defined above.} It is preferable that the polyimide precursor has a structural unit represented by the following formula:
[0025] In the general formula (9), at least one of R1 and R2 is more preferably a monovalent organic group represented by the above general formula (2). When the polyimide precursor (A) contains a polyimide precursor having a structural unit represented by general formula (9) in addition to the polyimide precursor having a structural unit represented by general formula (8), the effect of particularly improving the resolution is further improved.
[0026] From the viewpoints of chemical resistance, resolution, and suppression of voids after a high-temperature storage test, it is particularly preferable that (A) polyimide precursor is a mixture of a polyimide precursor having a structural unit represented by general formula (8) and a polyimide precursor having a structural unit represented by general formula (9), or a copolymer of the structural unit represented by general formula (8) and the structural unit represented by general formula (9). In general formulas (8) and (9), R1, R2, and n1 in one formula may be the same as or different from R1, R2, and n1 in the other formula, respectively.
[0027] (A) Method for preparing polyimide precursor (A) The polyimide precursor is obtained by first reacting a tetracarboxylic dianhydride containing the above-mentioned tetravalent organic group X1 with an alcohol having a photopolymerizable unsaturated double bond and, optionally, an alcohol having no unsaturated double bond to prepare a partially esterified tetracarboxylic acid (hereinafter, also referred to as an acid / ester body), and then subjecting this to amide polycondensation with a diamine containing the above-mentioned divalent organic group Y1.
[0028] (Preparation of Acid / Ester Forms) In the present embodiment, examples of the tetracarboxylic dianhydride containing a tetravalent organic group X1 that is suitably used for preparing the polyimide precursor (A) include the tetracarboxylic dianhydride represented by the above general formula (20), as well as, for example, pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyl tetracarboxylic dianhydride (BPDA), diphenyl sulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenyl methane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane. Preferred examples include pyromellitic anhydride, diphenylether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride (ODPA), and 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), but are not limited thereto. These may be used alone or in combination of two or more.
[0029] In the present embodiment, examples of alcohols having a photopolymerizable unsaturated double bond that are preferably used to prepare the polyimide precursor (A) include 2-hydroxyethyl methacrylate (HEMA), 2-acryloyloxyethyl alcohol, 1-acryloyloxy-3-propyl alcohol, 2-acrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-t-butoxypropyl acrylate, and 2-hydroxy-3-t-butoxypropyl acrylate. Examples of the hydroxypropyl acrylate include 2-hydroxy-3-cyclohexyloxypropyl acrylate, 2-methacryloyloxyethyl alcohol, 1-methacryloyloxy-3-propyl alcohol, 2-methacrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-t-butoxypropyl methacrylate, and 2-hydroxy-3-cyclohexyloxypropyl methacrylate.
[0030] The above-mentioned photopolymerizable alcohols having an unsaturated double bond may be partially mixed with alcohols not having an unsaturated double bond, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, neopentyl alcohol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 3-octanol, 1-nonanol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monomethyl ether, tetraethylene glycol monoethyl ether, and benzyl alcohol.
[0031] In addition, a non-photosensitive polyimide precursor prepared only from the alcohols not having an unsaturated double bond may be used as the polyimide precursor by mixing it with the photosensitive polyimide precursor. From the viewpoint of resolution, the non-photosensitive polyimide precursor is preferably 200 parts by mass or less based on 100 parts by mass of the photosensitive polyimide precursor.
[0032] The above-mentioned suitable tetracarboxylic dianhydride and the above-mentioned alcohol are stirred, dissolved, and mixed in a solvent as described below at a temperature of 20 to 50° C. for 4 to 10 hours in the presence of a basic catalyst such as pyridine, whereby the esterification reaction of the acid anhydride proceeds, and the desired acid / ester can be obtained.
[0033] (Preparation of polyimide precursor) The acid / ester (typically a solution in a solvent described below) is mixed with an appropriate dehydration condensation agent, such as dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, N,N'-disuccinimidyl carbonate, etc., under ice cooling to convert the acid / ester into a polyacid anhydride, and then a diamine containing a divalent organic group Y1 preferably used in this embodiment, dissolved or dispersed in a separate solvent, is added dropwise to the acid / ester to carry out amide polycondensation to obtain the desired polyimide precursor. Alternatively, the acid moiety of the acid / ester is converted into an acid chloride using thionyl chloride or the like, and then the acid is reacted with a diamine compound in the presence of a base such as pyridine to obtain the desired polyimide precursor.
[0034] Diamines containing a divalent organic group Y1 that are preferably used in this embodiment include diamines having a structure represented by the above general formula (21), as well as, for example, p-phenylenediamine, m-phenylenediamine, 4,4-diaminodiphenyl ether (4,4'-oxydianiline (ODA)), 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 3 ... ,4'-Diaminodiphenyl sulfone, 3,3'-Diaminodiphenyl sulfone, 4,4'-Diaminobiphenyl, 3,4'-Diaminobiphenyl, 3,3'-Diaminobiphenyl, 4,4'-Diaminobenzophenone, 3,4'-Diaminobenzophenone, 3,3'-Diaminobenzophenone, 4,4'-Diaminodiphenylmethane, 3,4'-Diaminodiphenylmethane, 3,3'-Diaminodiphenylmethane, 1,4-Bis(4-aminophenoxy)benzene, 1,3-Bis(4-aminophenoxy)benzene, 1,3-Bis(3-aminophenoxy) benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl) Propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, ortho-tolidine sulfone, 9,9-bis(4-aminophenyl)fluorene, and those in which some of the hydrogen atoms on the benzene ring are substituted with methyl groups, ethyl groups, hydroxymethyl groups, hydroxyethyl groups, halogens, etc., such as 3,3'-dimethyl-4,Examples of the diaminobiphenyl include, but are not limited to, 4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl (2,2'-dimethylbiphenyl-4,4'-diamine (m-TB)), 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 2,2'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethytoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, and mixtures thereof.
[0035] After the amide polycondensation reaction is completed, the water-absorbing by-product of the dehydration condensation agent coexisting in the reaction solution is filtered off as necessary, and then a poor solvent such as water, an aliphatic lower alcohol, or a mixture thereof is added to the resulting polymer component to precipitate the polymer component, and the polymer is purified by repeating redissolution and reprecipitation operations, and then vacuum drying is performed to isolate the desired polyimide precursor. In order to improve the degree of purification, the polymer solution may be passed through a column packed with an anion and / or cation exchange resin swollen with an appropriate organic solvent to remove ionic impurities.
[0036] The molecular weight of the polyimide precursor (A) is preferably 8,000 to 150,000, more preferably 9,000 to 50,000, when measured by gel permeation chromatography in terms of polystyrene equivalent weight average molecular weight. When the weight average molecular weight is 8,000 or more, the mechanical properties are good, and when it is 150,000 or less, the dispersibility in the developer is good, and the resolution performance of the relief pattern is good. As the developing solvent for gel permeation chromatography, tetrahydrofuran and N-methyl-2-pyrrolidone are recommended. The weight average molecular weight is obtained from a calibration curve prepared using standard monodisperse polystyrene. As the standard monodisperse polystyrene, it is recommended to select from the organic solvent-based standard sample STANDARD SM-105 manufactured by Showa Denko KK.
[0037] (B) Compounds having a urethane bond or a urea bond The compound (B) used in this embodiment contains at least one selected from a urethane bond and a urea bond in its molecular structure (hereinafter, in this embodiment, also referred to as a "urethane / urea compound"). The compound used in this embodiment is not limited to any other structure as long as it has a urethane bond and / or a urea bond in its molecular structure. Among these, it is preferable that the compound (B) has a urea bond from the viewpoint of suppressing Cu surface voids and chemical resistance. In this embodiment, it is preferable that the compound (B) further has at least one functional group selected from the group consisting of a (meth)acrylic group, a hydroxyl group, an alkoxy group, and an amino group.
[0038] Although the reason why the inclusion of the compound (B) according to the present embodiment results in good chemical resistance and resolution is not clear, the present inventors consider it as follows. That is, in one aspect, the negative photosensitive resin composition is heat-cured at a low temperature of 180° C. or less, so that the conversion of the polyimide precursor to polyimide tends to be insufficient. On the other hand, the negative photosensitive resin composition of the present embodiment contains the urethane / urea compound (B), so that a part of the compound (B) is thermally decomposed to generate amines, etc., which are believed to promote the conversion of the polyimide precursor to polyimide. In a preferred aspect, the compound (B) further has a (meth)acrylic group, and when the compound is made into a negative photosensitive resin composition, the compound (B) reacts with the side chain portion of the polyimide precursor by light irradiation to crosslink, so that the compound (B) is more likely to exist in the vicinity of the polyimide precursor, and the conversion efficiency can be dramatically improved.
[0039] In this embodiment, when the (B) compound further has a (meth)acrylic group, the (meth)acrylic equivalent of the (B) compound is preferably 150 to 400 g / mol. When the (meth)acrylic equivalent of the (B) compound is 150 g / mol or more, the chemical resistance of the negative photosensitive resin composition tends to be good, and when it is 400 g / mol or less, the developability tends to be good. The lower limit of the (meth)acrylic equivalent of the (B) compound is more preferably 200 g / mol or more, 210 g / mol or more, 220 g / mol or more, 230 g / mol or more, more preferably 240 g / mol or more, 250 g / mol or more, and the lower limit is more preferably 350 g / mol or less, 330 g / mol or less, and more preferably 300 g / mol or less. The (meth)acrylic equivalent of the (B) compound is even more preferably 210 to 400 g / mol, particularly preferably 220 to 400 g / mol.
[0040] The urethane / urea compound (B) used in the present embodiment is preferably a (meth)acrylic group-containing urethane / urea compound having a structure represented by the following general formula (3). [ka] {In the formula, R3 is a hydrogen atom or a methyl group, A is a group selected from the group consisting of -O-, -NH-, and -NL4-, L4 is a monovalent organic group having 1 to 12 carbon atoms, Z1 is an m2-valent organic group having 2 to 24 carbon atoms, Z2 is a divalent organic group having 2 to 8 carbon atoms, and m2 is an integer of 1 to 3.}
[0041] R3 is not limited as long as it is a hydrogen atom or a methyl group, but is preferably a methyl group from the viewpoint of developability. Z1 is not limited as long as it is an organic group having m2 valences of 2 to 20 carbon atoms. Here, Z1 may also contain heteroatoms such as oxygen atoms, sulfur atoms, nitrogen atoms, and phosphorus atoms. If Z1 has 2 or more carbon atoms, the negative photosensitive resin composition tends to have good chemical resistance, and if it has 20 or less carbon atoms, the developability tends to be good. The carbon number of Z1 is preferably 3 or more, more preferably 4 or more, and preferably 18 or less, and more preferably 16 or less. Z2 is not limited as long as it is a divalent organic group having 2 to 8 carbon atoms. Here, Z2 may also contain heteroatoms such as oxygen atoms, sulfur atoms, nitrogen atoms, and phosphorus atoms. If Z2 has 2 or more carbon atoms, the negative photosensitive resin composition tends to have good chemical resistance, and if it has 8 or less carbon atoms, the heat resistance tends to be good. The carbon number of Z2 is preferably 6 or less, more preferably 4 or less. A is a group selected from the group consisting of -O-, -NH-, and -NL4-. From the viewpoint of chemical resistance, A is preferably -NH- or -NL4-.
[0042] The method for producing the (meth)acrylic group-containing urea / urethane compound of the above general formula (3) is not particularly limited, but it can be obtained, for example, by reacting an isocyanate compound represented by the following general formula with an amine and / or a hydroxyl group-containing compound. [ka]
[0043] Among the compounds (B) described above, from the viewpoints of chemical resistance, void suppression, and developability, at least one compound selected from the group consisting of the following formulas (4) to (7) and (11) to (14) is particularly preferred. The compounds represented by the following formulas (4) to (7) and (11) to (14) are also one embodiment of the present invention. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0044] The urethane / urea compound (B) of this embodiment preferably further has at least one functional group selected from the group consisting of a hydroxyl group, an alkoxy group, and an amino group. The urethane / urea compound of this embodiment contains at least one functional group selected from the group consisting of a hydroxyl group, an alkoxy group, and an amino group, and thus tends to have good adhesion to the molded resin used in the fan-out type semiconductor package, which is one embodiment. The reason for this is not clear, but the present inventors believe it to be as follows. That is, in one embodiment, the negative photosensitive resin composition is heat-cured at a low temperature of 180° C. or less. At such a low temperature, the epoxy resin contained in the molded resin used in the fan-out type semiconductor package has an epoxy structure without being partially ring-opened, and the epoxy structure tends to interact with the hydroxyl group, alkoxy group, amino group, etc. contained in the urethane / urea compound (B). On the other hand, it is presumed that the urethane / urea structure contained in the compound (B) interacts with the polyimide resin, thereby exhibiting high adhesion to the molded resin. Among these functional groups, hydroxyl and alkoxy groups are preferred, and hydroxyl groups are particularly preferred. From the viewpoints of adhesion to the mold resin, chemical resistance, and suppression of Cu voids, the compound (B) more preferably has a (meth)acrylic group and a hydroxyl group in the molecular structure in addition to the urethane / urea structure.
[0045] The alkoxy group is more preferably an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, a propoxy group, etc. Examples of these compounds include compounds having the following structures. [ka] [ka] [ka]
[0046] In the present embodiment, the (B) compound may be used alone or in combination of two or more. The blending amount of the (B) compound is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the (A) polyimide precursor. The blending amount of the (B) is 0.1 parts by mass or more from the viewpoint of photosensitivity or patterning property, and is 30 parts by mass or less from the viewpoint of the physical properties of the photosensitive resin layer after curing of the negative photosensitive resin composition.
[0047] (C) Photopolymerization initiator The photopolymerization initiator is preferably a photoradical polymerization initiator. Examples of the photoradical polymerization initiator include benzophenone derivatives such as benzophenone, o-benzoyl methyl benzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, and fluorenone; acetophenone derivatives such as 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, and 1-hydroxycyclohexylphenyl ketone; thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone; benzyl derivatives such as benzil, benzil dimethyl ketal, and benzyl-β-methoxyethyl acetal; benzoin derivatives such as benzoin and benzoin methyl ether; 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl ) oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl) oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl) oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl) oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl) oxime, and 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl) oxime; N-arylglycines such as N-phenylglycine; peroxides such as benzoyl perchloride; aromatic biimidazoles; titanocenes; and photoacid generators such as α-(n-octanesulfonyloxyimino)-4-methoxybenzyl cyanide, but are not limited thereto. Among the above photopolymerization initiators, oximes are more preferable, particularly in terms of photosensitivity.
[0048] The amount of the photopolymerization initiator (C) is preferably 0.1 to 20 parts by mass, more preferably 1 to 8 parts by mass, based on 100 parts by mass of the polyimide precursor (A). The amount is 0.1 parts by mass or more from the viewpoint of photosensitivity or patterning property, and 20 parts by mass or less from the viewpoint of physical properties of the photosensitive resin layer after curing of the negative photosensitive resin composition.
[0049] (D) Rust inhibitor The negative photosensitive resin composition of the present embodiment may further include a rust inhibitor. The rust inhibitor is not limited as long as it can prevent metal from rusting, and may be a nitrogen-containing heterocyclic compound. Examples of the nitrogen-containing heterocyclic compound include an azole compound and a purine derivative.
[0050] Examples of the azole compounds include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, azole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, and 1-methyl-1H-tetrazole.
[0051] Particularly preferred examples of the azole compound include tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or in combination of two or more.
[0052] Purine derivatives include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, and 8-aminoadenine. Examples of the azaadenine include 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, and 8-azahypoxanthine, as well as derivatives thereof.
[0053] When the negative photosensitive resin composition contains an azole compound or a purine derivative, the blending amount is preferably 0.05 to 5 parts by mass relative to 100 parts by mass of the polyimide precursor (A), and more preferably 0.1 to 5 parts by mass from the viewpoint of photosensitivity characteristics. When the blending amount of the azole compound relative to 100 parts by mass of the polyimide precursor (A) is 0.05 parts by mass or more, when the negative photosensitive resin composition of this embodiment is formed on copper or a copper alloy, discoloration of the copper or copper alloy surface is suppressed, while when the azole compound is 5 parts by mass or less, the photosensitivity is excellent.
[0054] When the negative photosensitive resin composition of this embodiment contains (D) an anticorrosive agent, the formation of voids in the Cu layer is particularly suppressed. Although the reason for this effect is unclear, it is believed that the anticorrosive agent present on the Cu surface interacts with the (meth)acrylic group, hydroxyl group, alkoxy group, or amino group contained in the preferred embodiment of the urethane / urea compound to form a dense layer near the Cu interface.
[0055] (E) Silane coupling agent The negative photosensitive resin composition of the present embodiment may further contain a silane coupling agent. Examples of the silane coupling agent include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]propionate ... Examples of silane coupling agents include silane coupling agents such as [N-[3-triethoxysilyl]propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamido)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, N-phenylaminopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, and 3-(trialkoxysilyl)propyl succinic anhydride.
[0056] More specifically, the silane coupling agent may be 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name KBM803, manufactured by Chisso Corporation: trade name Sila-Ace S810), 3-mercaptopropyltriethoxysilane (manufactured by Azmax Corporation: trade name SIM6475.0), 3-mercaptopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS1375, manufactured by Azmax Corporation: trade name SIM6474.0), mercaptomethyltrimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.5C), mercaptomethylmethyldimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.0), 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyldiethoxymethoxysilane, 2-mercaptoethyl triethylethoxydimethoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltripropoxysilane, N-(3-triethoxysilylpropyl)urea (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name) LS3610, Azmax Corporation: Trade name SIU9055.0), N-(3-trimethoxysilylpropyl)urea (Azmax Corporation: Trade name SIU9058.0), N-(3-diethoxymethoxysilylpropyl)urea, N-(3-ethoxydimethoxysilylpropyl)urea, N-(3-tripropoxysilylpropyl)urea, N-(3-diethoxypropoxysilylpropyl)urea, N-(3-ethoxydipropoxysilylpropyl)urea, N-(3-dimethoxypropoxysilylpropyl)urea,N-(3-methoxydipropoxysilylpropyl)urea, N-(3-trimethoxysilylethyl)urea, N-(3-ethoxydimethoxysilylethyl)urea, N-(3-trippropoxysilylethyl)urea, N-(3-trippropoxysilylethyl)urea, N-(3-ethoxydipropoxysilylethyl)urea, N-(3-dimethoxypropoxysilylethyl)urea, N-(3-methoxydipropoxysilylethyl)urea, N-(3-trimethoxysilylbutyl)urea, N-(3-triethoxysilylbutyl)urea, N-(3-trippropoxysilylbutyl)urea, 3-(m-aminophenoxy)propyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0598.0), m-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.0), p-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.1) aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.2), 2-(trimethoxysilylethyl)pyridine (manufactured by Azmax Corporation: trade name SIT8396.0), 2-(triethoxysilylethyl)pyridine, 2-(dimethoxysilylmethylethyl)pyridine, 2-(diethoxysilylmethylethyl)pyridine, (3-triethoxysilylpropyl)-t-butylcarbamate, (3-glycidoxypropyl)triethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, tetrakis(methoxyethoxysilane), tetra tetrakis(methoxy-n-propoxysilane), tetrakis(ethoxyethoxysilane), tetrakis(methoxyethoxyethoxysilane), bis(trimethoxysilyl)ethane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)methane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)ethylene, bis(triethoxysilyl)octane, bis(triethoxysilyl)octadiene, bis[3-(triethoxysilyl)propyl]disulfide, bis[3-(triethoxysilyl)propyl]tetrasulfide,Di-t-butoxydiacetoxysilane, di-i-butoxyaluminoxytriethoxysilane, phenylsilanetriol, methylphenylsilanediol, ethylphenylsilanediol, n-propylphenylsilanediol, isopropylphenylsilanediol, n-butyldiphenylsilanediol, isobutylphenylsilanediol, tert-butylphenylsilanediol, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, ethylmethylphenylsilanol, n-propylmethylphenylsilanol, isopropylmethylphenylsilanol, n-butyl Examples of the silanol include, but are not limited to, methylphenylsilanol, isobutylmethylphenylsilanol, tert-butylmethylphenylsilanol, ethyl n-propylphenylsilanol, ethylisopropylphenylsilanol, n-butylethylphenylsilanol, isobutylethylphenylsilanol, tert-butylethylphenylsilanol, methyldiphenylsilanol, ethyldiphenylsilanol, n-propyldiphenylsilanol, isopropyldiphenylsilanol, n-butyldiphenylsilanol, isobutyldiphenylsilanol, tert-butyldiphenylsilanol, and triphenylsilanol. These may be used alone or in combination.
[0057] Among the above-mentioned silane coupling agents, from the viewpoint of storage stability, preferred silane coupling agents are phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and silane coupling agents having a structure represented by the following formula: [ka]
[0058] When a silane coupling agent is used, the amount of the silane coupling agent is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polyimide precursor (A). When the negative photosensitive resin composition of this embodiment contains a silane coupling agent (E), void formation in the Cu layer is particularly suppressed. Although the reason for this effect is unclear, it is believed that the silane coupling agent unevenly distributed on the Cu surface interacts with the (meth)acrylic group, hydroxyl group, alkoxy group, or amino group contained in the preferred embodiment of the urethane / urea compound to form a dense layer near the Cu interface.
[0059] (F) Other Ingredients The negative type photosensitive resin composition of the present embodiment may further contain components other than the above components (A) to (E). The components other than the components (A) to (E) include, but are not limited to, a solvent, a hindered phenol compound, an organic titanium compound, a sensitizer, a photopolymerizable unsaturated monomer, a thermal polymerization inhibitor, and the like.
[0060] solvent Examples of the solvent include amides, sulfoxides, ureas, ketones, esters, lactones, ethers, halogenated hydrocarbons, hydrocarbons, and alcohols. More specifically, for example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, tetramethylurea, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethyl lactate, methyl lactate, butyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, benzyl alcohol, phenyl glycol, tetrahydrofurfuryl alcohol, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, morpholine, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, anisole, hexane, heptane, benzene, toluene, xylene, mesitylene, and the like can be used. Among these, from the viewpoints of the solubility of the resin, the stability of the resin composition, and the adhesion to the substrate, N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetramethylurea, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, diethylene glycol dimethyl ether, benzyl alcohol, phenyl glycol, and tetrahydrofurfuryl alcohol are preferred.
[0061] Among these solvents, those which completely dissolve the produced polymer are particularly preferred, and examples thereof include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, tetramethylurea, and gamma-butyrolactone.
[0062] In the negative type photosensitive resin composition of the present embodiment, the amount of the solvent used is preferably 100 to 1,000 parts by mass, more preferably 120 to 700 parts by mass, and even more preferably 125 to 500 parts by mass, relative to 100 parts by mass of the polyimide precursor (A).
[0063] Hindered phenol compounds In order to suppress discoloration on the copper surface, the negative photosensitive resin composition may optionally contain a hindered phenol compound. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenon), and the like. ol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylphenol) 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4,6 -(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl )-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-to 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine Examples of the triazine include, but are not limited to, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and the like. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione and the like are particularly preferred.
[0064] The amount of the hindered phenol compound is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polyimide precursor (A), and from the viewpoint of photosensitivity characteristics, more preferably 0.5 to 10 parts by mass. When the amount of the hindered phenol compound is 0.1 part by mass or more relative to 100 parts by mass of the polyimide precursor (A), for example, when the photosensitive resin composition of the present invention is formed on copper or a copper alloy, discoloration and corrosion of the copper or copper alloy are prevented, while when the amount is 20 parts by mass or less, excellent photosensitivity is achieved.
[0065] Organotitanium Compounds The negative photosensitive resin composition of the present embodiment may contain an organotitanium compound. By containing an organotitanium compound, a photosensitive resin layer having excellent chemical resistance can be formed even when cured at a low temperature.
[0066] Usable organotitanium compounds include those in which an organic chemical is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organotitanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Among these, titanium chelates having two or more alkoxy groups are more preferred because they provide good storage stability and a good pattern for the negative photosensitive resin composition. Specific examples include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), etc. II) Tetraalkoxytitanium compounds: For example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], and the like. III) Titanocene compounds: For example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like. IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc. V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, and the like. VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate. VII) Titanate coupling agents: For example, isopropyl tridodecylbenzenesulfonyl titanate.
[0067] Among them, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium are preferred.
[0068] When an organic titanium compound is blended, the blending amount is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the polyimide precursor (A). When the blending amount of the organic titanium compound is 0.05 parts by mass or more, good heat resistance and chemical resistance are exhibited, while when it is 10 parts by mass or less, excellent storage stability is obtained.
[0069] Sensitizer The negative photosensitive resin composition of the present embodiment may optionally contain a sensitizer to improve photosensitivity. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylideneindanone, and the like. p-Dimethylaminobenzylideneindanone, 2-(p-Dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-Dimethylaminophenylvinylene)benzothiazole, 2-(p-Dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetate Examples of the mercaptobenzoyl compounds include 1-phenyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, and 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, and 2-(p-dimethylaminobenzoyl)styrene. These may be used alone or in combination of two or more, for example, two to five types.
[0070] When the photosensitive resin composition contains a sensitizer, the amount of the sensitizer is preferably 0.1 to 25 parts by mass per 100 parts by mass of the (A) polyimide precursor.
[0071] Photopolymerizable Unsaturated Monomers The negative photosensitive resin composition may optionally contain a monomer having a photopolymerizable unsaturated bond (photopolymerizable unsaturated monomer) in order to improve the resolution of the relief pattern. As such a monomer, a (meth)acrylic compound that undergoes a radical polymerization reaction with a photopolymerization initiator is preferable, and examples thereof include, but are not limited to, mono- or diacrylates and methacrylates of ethylene glycol or polyethylene glycol, such as diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, mono- or diacrylates and methacrylates of propylene glycol or polypropylene glycol, mono-, di- or triacrylates and methacrylates of glycerol, cyclohexane diacrylate and dimethacrylate, diacrylates and dimethacrylates of 1,4-butanediol, and 1,6-hexane diacrylate and dimethacrylate. Examples of such compounds include diacrylates and dimethacrylates of diols, diacrylates and dimethacrylates of neopentyl glycol, mono- or diacrylates and methacrylates of bisphenol A, benzene trimethacrylate, isobornyl acrylate and methacrylate, acrylamide and its derivatives, methacrylamide and its derivatives, trimethylolpropane triacrylate and methacrylate, di- or triacrylates and methacrylates of glycerol, di-, tri-, or tetraacrylates and methacrylates of pentaerythritol, and ethylene oxide or propylene oxide adducts of these compounds.
[0072] When the photosensitive resin composition contains a photopolymerizable unsaturated monomer, the amount of the monomer is preferably 1 to 50 parts by mass per 100 parts by mass of the polyimide precursor (A).
[0073] Thermal Polymerization Inhibitor The negative photosensitive resin composition of the present embodiment may optionally contain a thermal polymerization inhibitor in order to improve the stability of the viscosity and photosensitivity of the negative photosensitive resin composition during storage, particularly in the form of a solution containing a solvent. Examples of the thermal polymerization inhibitor include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0074] <Method for Producing Cured Relief Pattern and Semiconductor Device> The method for producing a cured relief pattern of the present embodiment includes the steps of: (1) applying the negative type photosensitive resin composition of the present embodiment onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat-treating the relief pattern to form a hardened relief pattern.
[0075] (1) Photosensitive resin layer formation process In this step, the negative photosensitive resin composition of the present embodiment is applied onto a substrate, and then dried as necessary to form a photosensitive resin layer. As the application method, a method that has been conventionally used for applying a photosensitive resin composition, such as a method of applying with a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, etc., and a method of spray application with a spray coater, etc., can be used.
[0076] If necessary, the coating film containing the photosensitive resin composition can be dried. As a drying method, air drying, heat drying using an oven or a hot plate, vacuum drying, etc. can be used. Specifically, when air drying or heat drying is performed, drying can be performed under conditions of 20°C to 140°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on the substrate.
[0077] (2) Exposure process In this step, the photosensitive resin layer formed above is exposed to an ultraviolet light source or the like. For the exposure method, an exposure device such as a contact aligner, a mirror projection, or a stepper can be used. The exposure can be performed directly or through a photomask or reticle having a pattern.
[0078] Thereafter, for the purpose of improving the photosensitivity, etc., a post-exposure bake (PEB) and / or a pre-development bake may be performed at any combination of temperature and time, as necessary. The range of baking conditions is preferably a temperature of 40° C. to 120° C. and a time of 10 seconds to 240 seconds, but is not limited to this range as long as it does not impair the various properties of the photosensitive resin composition of the present invention.
[0079] (3) Relief pattern formation process In this process, the unexposed portion of the exposed photosensitive resin layer is developed and removed from the substrate, leaving a relief pattern on the substrate. As a development method for developing the exposed (irradiated) photosensitive resin layer, any method can be selected from conventionally known photoresist development methods, such as a rotary spray method, a paddle method, and an immersion method accompanied by ultrasonic treatment. After development, post-development baking may be performed at any combination of temperature and time, if necessary, for the purpose of adjusting the shape of the relief pattern.
[0080] The developer used for development is preferably, for example, a good solvent for the negative photosensitive resin composition, or a combination of the good solvent and a poor solvent. As the good solvent, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone are preferred. As the poor solvent, for example, toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, and water are preferred. When a good solvent and a poor solvent are used in combination, it is preferred to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the negative photosensitive resin composition. Also, two or more types of each solvent, for example, several types, can be used in combination.
[0081] (4) Hardened relief pattern formation process In this step, the relief pattern obtained by the above development is heated to disperse the photosensitive component and imidize the polyimide precursor (A), thereby converting it into a cured relief pattern made of polyimide. As a method for heat curing, various methods can be selected, such as a method using a hot plate, an oven, or a method using a temperature-elevating oven that can set a temperature program. Heating can be performed, for example, under conditions of 170°C to 400°C for 30 minutes to 5 hours. As the atmospheric gas during heat curing, air may be used, or an inert gas such as nitrogen or argon may also be used.
[0082] <Polyimide> The structure of the polyimide contained in the cured relief pattern formed from the polyimide precursor composition is represented by the following general formula (10). [ka] {In general formula (10), X 1 and Y 1 are the same as X1 and Y1 in general formula (1), and m is a positive integer.
[0083] For the same reason, the preferred X1 and Y1 in general formula (1) are also preferred in the polyimide of general formula (10). The number m of repeating units in general formula (10) is not particularly limited, but may be an integer of 2 to 150. In addition, a method for producing a polyimide including a step of converting the above-described negative photosensitive resin composition into a polyimide is also one aspect of the present invention.
[0084] <Semiconductor device> In this embodiment, a semiconductor device having a cured relief pattern obtained by the above-mentioned method for producing a cured relief pattern is also provided. Thus, a semiconductor device can be provided having a substrate that is a semiconductor element and a cured relief pattern of polyimide formed on the substrate by the above-mentioned method for producing a cured relief pattern. The present invention can also be applied to a method for producing a semiconductor device that uses a semiconductor element as the substrate and includes the above-mentioned method for producing a cured relief pattern as part of the process. The semiconductor device of the present invention can be produced by forming the cured relief pattern formed by the above-mentioned method for producing a cured relief pattern as a surface protective film, an interlayer insulating film, an insulating film for rewiring, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure, and combining the method with a known method for producing a semiconductor device.
[0085] <Display device> In this embodiment, a display device is provided that includes a display element and a cured film provided on the upper portion of the display element, and the cured film is the above-mentioned cured relief pattern. Here, the cured relief pattern may be laminated in direct contact with the display element, or may be laminated with another layer sandwiched therebetween. For example, the cured film may be a surface protective film, an insulating film, and a planarizing film for a TFT liquid crystal display element and a color filter element, a protrusion for an MVA type liquid crystal display device, and a partition wall for a cathode of an organic EL element.
[0086] The negative photosensitive resin composition of the present invention is useful not only for application to the semiconductor device described above, but also for applications such as interlayer insulation in multilayer circuits, cover coats for flexible copper-clad boards, solder resist films, and liquid crystal alignment films. EXAMPLES
[0087] The present embodiment will be described in detail below with reference to examples, but the present embodiment is not limited thereto. In the examples, comparative examples, and production examples, the physical properties of the polymer or the negative photosensitive resin composition were measured and evaluated according to the following methods.
[0088] <Measurement and evaluation methods> (1) Weight average molecular weight The weight average molecular weight (Mw) of each resin was measured using gel permeation chromatography (standard polystyrene equivalent) under the following conditions. Pump: JASCO PU-980 Detector: JASCO RI-930 Column oven: JASCO CO-965 40℃ Column: Showa Denko Shodex KD-806M, 2 in series, or Showa Denko Shodex 805M / 806M series Standard monodisperse polystyrene: Showa Denko Co., Ltd. Shodex STANDARD SM-105 Mobile phase: 0.1 mol / L LiBr / N-methyl-2-pyrrolidone (NMP) Flow rate: 1mL / min
[0089] (2) Fabrication of hardened relief patterns on Cu A 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) was sputtered with 200 nm of Ti and 400 nm of Cu, in that order, using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Next, a negative-type photosensitive resin composition prepared by the method described below was spin-coated on this wafer using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.), and prebaked on a hot plate at 110°C for 180 seconds to form a coating film with a thickness of approximately 7 μm. Using a test pattern mask, this coating film was then sprayed with 500 mJ / cm using Prisma GHI (manufactured by Ultratech Co., Ltd.). 2The coating was then spray-developed with a coater developer (D-Spin60A, manufactured by SOKUDO) using cyclopentanone as a developer, and rinsed with propylene glycol methyl ether acetate to obtain a relief pattern on Cu. The wafer on which the relief pattern was formed on Cu was heat-treated for 2 hours in a nitrogen atmosphere at the curing temperature shown in Table 1 using a temperature-programmable curing furnace (VF-2000, manufactured by Koyo Lindberg) to obtain a cured relief pattern made of resin with a thickness of about 4 to 5 μm on Cu.
[0090] (3) Resolution evaluation of hardened relief patterns on Cu The cured relief pattern obtained by the above method was observed under an optical microscope to determine the size of the minimum opening pattern. At this time, if the area of the opening of the obtained pattern was 1 / 2 or more of the corresponding pattern mask opening area, it was considered to be resolved, and the length of the mask opening side corresponding to the smallest area among the resolved openings was taken as the resolution. Resolutions less than 10 μm were rated as "excellent," those between 10 μm and 14 μm as "good," those between 14 μm and 18 μm as "fair," and those over 18 μm as "poor."
[0091] (4) High temperature storage test of hardened relief patterns on Cu and subsequent evaluation of Cu surface void area The wafer with the cured relief pattern formed on Cu was heated in air at 150°C for 168 hours using a temperature-programmable curing furnace (VF-2000, manufactured by Koyo Lindberg). Then, the resin layer on Cu was entirely removed by plasma etching using a plasma surface treatment device (EXAM, manufactured by Shinko Seiki Co., Ltd.). The plasma etching conditions were as follows: Output: 133W Gas type / flow rate: O2: 40mL / min + CF4: 1mL / min Gas pressure: 50Pa Mode: Hard Mode Etching time: 1800 seconds The Cu surface from which the resin layer had been completely removed was observed with an FE-SEM (S-4800 model, Hitachi High-Technologies Corporation), and the area of voids on the surface of the Cu layer was calculated using image analysis software (Azo-kun, Asahi Kasei Corporation). When the total area of voids in the evaluation of the negative photosensitive resin composition described in Comparative Example 1 was taken as 100%, those with a total void area ratio of less than 50% were judged as "excellent", those with a void area ratio of 50% or more but less than 75% were judged as "good", those with a void area ratio of 75% or more but less than 100% were judged as "passable", and those with a void area ratio of 100% or more were judged as "unacceptable".
[0092] (5) Chemical resistance evaluation of cured relief pattern (polyimide coating) The cured relief pattern formed on Cu was immersed in a resist stripper {manufactured by ATMI, product name ST-44, main components are 2-(2-aminoethoxy)ethanol, 1-cyclohexyl-2-pyrrolidone} heated to 50°C for 5 minutes, washed with running water for 1 minute, and air-dried. Thereafter, the film surface was visually observed with an optical microscope to evaluate the chemical resistance based on the presence or absence of damage caused by the chemical solution, such as cracks, and the change in film thickness after chemical treatment. As evaluation criteria, a film without cracks and a film thickness change rate of 10% or less based on the film thickness before chemical immersion was rated as "excellent", a film with a film thickness change rate of more than 10% to 15% or less was rated as "good", a film with a film thickness change rate of more than 15% to 20% was rated as "passable", and a film with cracks or a film thickness change rate of more than 20% was rated as "unacceptable".
[0093] (6) Adhesion test with sealing material As an epoxy-based encapsulant, the R4000 series manufactured by Nagase Chemtex Corporation was prepared. The encapsulant was spin-coated onto an aluminum-sputtered silicon wafer to a thickness of approximately 150 microns, and then thermally cured at 130°C to harden the epoxy-based encapsulant. The photosensitive resin composition prepared in each Example and Comparative Example was applied onto the above-mentioned epoxy-based cured film to a final film thickness of 10 microns. The applied photosensitive resin composition was exposed to light at a dose of 600 mJ / cm using an aligner (PLA-501F, manufactured by Canon Inc.). 2 The entire surface was exposed to Ghi rays. Then, it was thermally cured at 180°C for 2 hours to form a first layer of a cured film with a thickness of 10 microns.
[0094] The photosensitive resin composition used in forming the first cured film was applied onto the first cured film, and the entire surface was exposed to light under the same conditions as when the first cured film was prepared, and then the film was thermally cured to prepare a second cured film having a thickness of 10 microns. A pin was placed on the sample prepared in the encapsulant deterioration test, and an adhesion test was performed using a pull tester (Quad Group, Sebastian 5 type). That is, the adhesive strength between the epoxy encapsulant and the cured relief pattern prepared from the photosensitive resin composition prepared in each Example and Comparative Example was measured and evaluated according to the following criteria. Evaluation: Adhesive strength 70MPa or more...Adhesion A Adhesive strength: 50MPa or more - less than 70MPa...Adhesion strength B Adhesive strength: 30MPa or more - less than 50MPa...Adhesion strength C Adhesive strength: less than 30MPa Adhesion strength: D
[0095] Production Example 1: (A) Synthesis of Polymer A-1 as a Polyimide Precursor 155.1g of 4,4'-oxydiphthalic dianhydride (ODPA) was placed in a 2L separable flask, 131.2g of 2-hydroxyethyl methacrylate (HEMA) and 400mL of γ-butyrolactone were added and stirred at room temperature, and 81.5g of pyridine was added while stirring to obtain a reaction mixture. After the end of the heat generation due to the reaction, the reaction mixture was allowed to cool to room temperature and left for 16 hours. Next, under ice cooling, a solution obtained by dissolving 206.3g of dicyclohexylcarbodiimide (DCC) in 180mL of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring, followed by the addition of 93.0g of 4,4'-oxydianiline (ODA) suspended in 350mL of γ-butyrolactone over 60 minutes while stirring. After further stirring at room temperature for 2 hours, 30mL of ethyl alcohol was added and stirred for 1 hour, and then 400mL of γ-butyrolactone was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution. The reaction solution obtained was added to 3 L of ethyl alcohol to produce a precipitate consisting of a crude polymer. The crude polymer formed was filtered off and dissolved in 1.5 L of tetrahydrofuran to obtain a crude polymer solution. The crude polymer solution obtained was dropped into 28 L of water to precipitate the polymer, and the precipitate obtained was filtered off and then vacuum dried to obtain a powdered polymer (polymer A-1). The molecular weight of polymer (A-1) was measured by gel permeation chromatography (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 20,000.
[0096] Production Example 2: (A) Synthesis of Polymer A-2 as a Polyimide Precursor Polymer (A-2) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that 147.1 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) was used instead of 155.1 g of 4,4'-oxydiphthalic dianhydride (ODPA) in Production Example 1. The molecular weight of polymer (A-2) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 22,000.
[0097] Production Example 3: (A) Synthesis of Polymer A-3 as a Polyimide Precursor Polymer (A-3) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that 98.6 g of 2,2'-dimethylbiphenyl-4,4'-diamine (m-TB) was used instead of 93.0 g of 4,4'-oxydianiline (ODA) in Production Example 1. The molecular weight of polymer (A-3) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 21,000.
[0098] Production Example 4: (A) Synthesis of Polymer A-4 as a Polyimide Precursor Polymer (A-3) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that p-phenylenediamine (50.3 g) was used instead of 4,4'-oxydianiline (ODA) in Production Example 1. The molecular weight of polymer (A-3) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 18,000.
[0099] <Example 1> Method for producing MOI-D (Compound B-1) 55.1g (0.25mol) of diethylene glycol bis(3-aminopropyl) ether was placed in a 500mL separable flask, and 150mL of tetrahydrofuran was added and stirred at room temperature. Next, under ice cooling, a solution of 77.6g (0.50mol) of 2-methacryloyloxyethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz MOI) and 150mL of tetrahydrofuran was added dropwise to the flask over 30 minutes and stirred at room temperature for 5 hours. Then, tetrahydrofuran was distilled off using a rotary evaporator to obtain compound B-1. The methacrylic equivalent of compound B-1 was 265g / mol.
[0100] Example 2: Method for producing MOI-AP (Compound B-2) Compound B-2 was obtained by synthesizing in the same manner as in Example 1, except that 55.1 g of diethylene glycol bis(3-aminopropyl) ether was replaced with 51.1 g (0.25 mol) of 1,4-butanediol bis(3-aminopropyl ether). The methacrylic equivalent of compound B-2 was 257 g / mol.
[0101] Example 3: Method for producing MOI-ODA (Compound B-3) Compound B-3 was obtained by synthesizing in the same manner as in Example 1, except that 55.1 g of diethylene glycol bis(3-aminopropyl) ether was replaced with 50.1 g (0.25 mol) of ODA. The methacrylic equivalent of compound B-3 was 255 g / mol.
[0102] <Example 4> Method for producing MOI-DEtA (Compound B-4) Compound B-4 was obtained by synthesizing in the same manner as in Example 1, except that 55.1 g of diethylene glycol bis(3-aminopropyl) ether was replaced with 26.3 g (0.25 mol) of diethanolamine and 77.6 g of 2-methacryloyloxyethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz MOI) was replaced with 38.8 g (0.25 mol). The methacrylic equivalent of compound B-4 was 260 g / mol.
[0103] <Example 5> Manufacturing method of MOI-EG-MOI (Compound B-5) Compound B-5 was obtained by synthesizing in the same manner as in Example 1, except that 77.6 g of 2-methacryloyloxyethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz MOI) was replaced with 99.6 g (0.50 mol) of 2-(2-isocyanatoethyloxy)ethyl methacrylate. The methacrylic equivalent of compound B-5 was 309 g / mol.
[0104] Example 6: Method for producing MOI-DEA (Compound B-6) 55.1g (0.25mol) of N-phenyldiethanolamine was placed in a 500mL three-necked eggplant flask, and 100mL of propylene glycol monomethyl ether acetate was added and stirred at room temperature. Furthermore, 150mL of propylene glycol monomethyl ether acetate was added to 77.6g (0.50mol) of 2-methacryloyloxyethyl isocyanate (Showa Denko product, product name: Karenz MOI). Then, the flask was heated to 120°C in an oil bath, stirred at 120°C for 13 hours, and then cooled to room temperature. Then, propylene glycol monomethyl ether acetate was distilled off using a rotary evaporator to obtain compound B-6. The methacrylic equivalent of compound B-6 was 245g / mol.
[0105] <Example 7> Method for producing MOI-AEE (Compound B-7) In the above Production Example 5, 55.1 g of diethylene glycol bis(3-aminopropyl) ether was replaced with 26.3 g (0.25 mol) of 2-(2-aminoethoxy)ethanol, and 77.6 g of 2-methacryloyloxyethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz MOI) was replaced with 38.8 g (0.25 mol), but the synthesis was carried out in the same manner as in Example 1 to obtain compound B-7. The methacrylic equivalent of compound B-7 was 260 g / mol.
[0106] <Example 8> Manufacturing method of MOI-DOA (Compound B-8) In the above Example 1, 55.1 g of diethylene glycol bis(3-aminopropyl) ether was replaced with 60.4 g (0.25 mol) of di-n-octylamine, and 77.6 g of 2-methacryloyloxyethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz MOI) was replaced with 38.8 g (0.25 mol), but the synthesis was carried out in the same manner as in Example 1 to obtain compound B-8. The methacrylic equivalent of compound B-8 was 397 g / mol.
[0107] <Example 9> Method for producing BEI-DEtA (Compound B-9) 26.3g (0.25mol) of diethanolamine was placed in a 500mL separable flask, 150mL of tetrahydrofuran was added, and the mixture was stirred at room temperature. Next, under ice cooling, a solution of 59.8g (0.25mol) of 1,1-(bisacryloyloxymethyl)ethyl isocyanate (Showa Denko Co., Ltd., product name: Karenz BEI) and 150mL of tetrahydrofuran was added dropwise to the flask over 30 minutes, and the mixture was stirred at room temperature for 5 hours. Then, tetrahydrofuran was distilled off using a rotary evaporator to obtain compound B-9. The acrylic equivalent of compound B-9 was 172g / mol.
[0108] <Example 10> Preparation of BEI-BHEA (Compound B-10) Compound B-10 was obtained by synthesizing in the same manner as in Example 9, except that 26.3 g (0.25 mol) of diethanolamine was replaced with 37.1 g (0.25 mol) of N,N'-bis(2-hydroxyethyl)ethylenediamine and 59.8 g (0.25 mol) of 1,1-(bisacryloyloxymethyl)ethyl isocyanate was replaced with 119.6 g (0.50 mol). The acrylic equivalent of compound B-10 was 157 g / mol.
[0109] <Example 11> (Compound B-11) 2.10g (0.020mol) of diethanolamine was put into a 100mL three-neck flask, 5.6g of tetrahydrofuran was put in, and the mixture was stirred at room temperature. Next, under ice cooling, a solution of 2.67g (0.021mol) of hexyl isocyanate and 5.6g of tetrahydrofuran was added dropwise to the flask over 15 minutes, and the mixture was stirred at room temperature for 4 hours. Then, tetrahydrofuran was distilled off using a rotary evaporator, and compound B-11 was obtained.
[0110] <Example 12> (Compound B-12) Compound B-12 was obtained by the same synthesis method as in Example 11 above, except that 2.10 g (0.020 mol) of diethanolamine was replaced with 2.10 g (0.020 mol) of 2-(2-aminoethoxy)ethanol.
[0111] <Example 13> (Compound B-13) Compound B-13 was obtained by the same synthesis method as in Example 11, except that 2.10 g (0.020 mol) of diethanolamine was replaced with 2.66 g (0.020 mol) of bis(2-methoxyethyl)amine.
[0112] <Example 14> A negative photosensitive resin composition was prepared using polymer A-1 by the following method, and the prepared composition was evaluated. (A) 100 g of polymer A-1 as a polyimide precursor, (B) 8 g of compound B-1 of Example 1 as a compound, and (C) 3 g of ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (OXE-02, corresponding to photosensitizer C-1) as a photopolymerization initiator were dissolved in 150 g of γ-butyrolactone (GBL). The viscosity of the obtained solution was adjusted to about 30 poise by further adding a small amount of GBL to obtain a negative photosensitive resin composition. The composition was evaluated according to the above-mentioned method. The results are shown in Table 1.
[0113] <Examples 15 to 26> A negative photosensitive resin composition was prepared in the same manner as in Example 14, except that it was prepared in the blending ratio shown in Table 1, and was evaluated according to the above-mentioned method. The results are shown in Table 1.
[0114] <Example 27> Negative photosensitive resin compositions were prepared using polymers A-1 and A-2 by the following method, and the prepared compositions were evaluated. (A) 50 g of polymer A-1 and 50 g of polymer A-2 as polyimide precursors, (B) 8 g of compound B-1 as a compound, and (C) 3 g of ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (OXE-02, corresponding to photosensitizer C-1) as a photopolymerization initiator were dissolved in 150 g of γ-butyrolactone (GBL). The viscosity of the obtained solution was adjusted to about 30 poise by further adding a small amount of GBL to obtain a negative photosensitive resin composition. The composition was evaluated according to the above-mentioned method. The results are shown in Table 2.
[0115] <Examples 28 to 36> A negative photosensitive resin composition was prepared in the same manner as in Example 14, except that it was prepared in the blending ratio shown in Table 2, and was evaluated according to the above-mentioned method. The results are shown in Table 1.
[0116] <Example 37> A negative photosensitive resin composition was prepared using polymer A-3 by the following method, and the prepared composition was evaluated. (A) 100 g of polymer A-3 as a polyimide precursor, (B) 8 g of compound B-1 as a compound, and (C) 3 g of ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (OXE-02, corresponding to photosensitizer C-1) as a photopolymerization initiator were dissolved in 150 g of γ-butyrolactone (GBL). The viscosity of the obtained solution was adjusted to about 30 poise by further adding a small amount of GBL to obtain a negative photosensitive resin composition. The composition was evaluated according to the above-mentioned method. The results are shown in Table 2.
[0117] <Example 38> A negative photosensitive resin composition was produced in the same manner as in Example 24, except that Polymer A-4 was used instead of Polymer A-3, and was evaluated according to the above-mentioned method. The results are shown in Table 2.
[0118] <Comparative Example 1> A negative photosensitive resin composition was produced in the same manner as in Example 1, except that no compound (B) was used, and was evaluated according to the above-mentioned method. The results are shown in Table 2.
[0119] The compounds (B-1 to B-13) and the photosensitizer (C-1) shown in Table 1 are the following compounds.
[0120] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0121] C-1: Ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (trade name: IRGACURE OXE-02 (OXE-02))
[0122] [Table 1]
[0123] [Table 2] [Industrial Applicability]
[0124] By using the negative photosensitive resin composition according to the present invention, a cured relief pattern having high chemical resistance and resolution can be obtained, and the generation of voids on the Cu surface can be suppressed. The present invention can be suitably used in the field of photosensitive materials useful for manufacturing electric and electronic materials such as semiconductor devices and multilayer wiring boards.
Claims
1. (A) a polyimide precursor represented by the following general formula (1): (B) a compound containing a (meth)acrylic group and a urea bond; and (C) Photopolymerization initiator A negative type photosensitive resin composition comprising: The compound (B) is a negative type photosensitive resin composition having a structure obtained by reacting an isocyanate compound with an amine-containing compound. 【Chemistry 1】 {In the formula, X 1 is a tetravalent organic group, Y 1 is a divalent organic group, n 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group; R 1 and R 2 At least one of the groups is a monovalent organic group represented by the following general formula (2): 【Chemistry 2】 {In the formula, L 1 , L 2 and L 3 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms, and m 1 is an integer from 2 to 10.
2. The negative type photosensitive resin composition according to claim 1 , wherein the compound (B) further contains at least one functional group selected from a hydroxyl group, an alkoxy group, and an amino group.
3. 2. The negative type photosensitive resin composition according to claim 1, wherein the compound (B) has a (meth)acrylic equivalent of 150 to 400 g / mol.
4. The negative type photosensitive resin composition according to claim 1 , wherein the compound (B) further contains a hydroxyl group.
5. The negative type photosensitive resin composition according to any one of claims 1 to 4, wherein the compound (B) has a structure represented by the following general formula (3): 【Chemistry 3】 {In the formula, R 3 is a hydrogen atom or a methyl group, and A is -NH- or -NL 4 -, and L 4 is a monovalent organic group having 1 to 12 carbon atoms; Z 1 m is a carbon number of 2 to 24 2 is a 4-valent organic group, 2 is a divalent organic group having 2 to 8 carbon atoms, and m 2 is an integer from 1 to 3.
6. The negative type photosensitive resin composition according to any one of claims 1 to 5, further comprising (D) a rust inhibitor.
7. The negative type photosensitive resin composition according to claim 6 , wherein the (D) rust inhibitor comprises a nitrogen-containing heterocyclic compound.
8. The negative type photosensitive resin composition according to claim 7 , wherein the nitrogen-containing heterocyclic compound is an azole compound.
9. The negative type photosensitive resin composition according to claim 7 , wherein the nitrogen-containing heterocyclic compound is a purine derivative.
10. The negative type photosensitive resin composition according to any one of claims 1 to 9, further comprising (E) a silane coupling agent.
11. The negative type photosensitive resin composition according to any one of claims 1 to 10, wherein X1 in the polyimide precursor (A) includes at least one selected from the group consisting of the following general formulas (20a), (20b), and (20c): 【Chemistry 4】 【Chemistry 5】 【Chemistry 6】 In the formula, R6 is independently a hydrogen atom, a fluorine atom, 1 ~C 10 and C 1 ~C 10 where l is an integer selected from 0 to 2, and m is an integer selected from 0 to 3.
12. The negative type photosensitive resin composition according to any one of claims 1 to 11, wherein Y1 in the polyimide precursor (A) includes at least one selected from the group consisting of the following general formulas (21a), (21b), and (21c): 【Chemistry 7】 【Chemistry 8】 【Chemistry 9】 In the formula, R6 is independently a hydrogen atom, a fluorine atom, 1 ~C 10 and C 1 ~C 10 and n is an integer selected from 0 to 4.
13. The polyimide precursor (A) is represented by the following general formula (8): 【Chemistry 10】 {In the formula, n 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group. The negative type photosensitive resin composition according to any one of claims 1 to 12, comprising a polyimide precursor having a structural unit represented by the following formula:
14. The polyimide precursor (A) is represented by the following general formula (9): 【Chemistry 11】 {In the formula, n 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group. The negative type photosensitive resin composition according to any one of claims 1 to 13, comprising a polyimide precursor having a structural unit represented by the following formula:
15. The polyimide precursor (A) is represented by the following general formula (8): 【Chemistry 12】 {In the formula, n 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group, and R in the general formula (9) 1 , R 2 , and n 1 may be the same as or different from. A structural unit represented by The following general formula (9): 【Chemistry 13】 {In the formula, n 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group, and R in the general formula (8) 1 , R 2 , and n 1 may be the same as or different from. or a copolymer with a structural unit represented by The negative type photosensitive resin composition according to any one of claims 1 to 14, which is a mixture of a polyimide precursor having a structural unit represented by the general formula (8) and a polyimide precursor having a structural unit represented by the general formula (9).
16. 16. The negative type photosensitive resin composition according to claim 15, wherein the polyimide precursor (A) is a copolymer of a structural unit represented by the general formula (8) and a structural unit represented by the general formula (9).
17. 100 parts by mass of the polyimide precursor (A); 0.1 to 30 parts by mass of the (B) compound based on 100 parts by mass of the (A) polyimide precursor; 0.1 to 20 parts by mass of the photopolymerization initiator (C) based on 100 parts by mass of the polyimide precursor (A); The negative type photosensitive resin composition according to any one of claims 1 to 16, comprising:
18. A method for producing a polyimide, comprising a step of converting the negative type photosensitive resin composition according to any one of claims 1 to 17 into a polyimide.
19. (1) applying the negative type photosensitive resin composition according to any one of claims 1 to 17 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising:
Citation Information
Patent Citations
Flip chip type semiconductor device and its manufacturing method
JP2001338947A
Aqueous gel and production method therefor
JP2016210912A