Isocyanate composition, coating composition, coating film and coated article
The isocyanate composition, combining triisocyanate and p-toluenesulfonyl isocyanate, addresses the issues of viscosity stability and solvent resistance in coating films, enhancing drying properties and reducing yellowing.
Patent Information
- Application Number
- JP2018137933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-07-24
- Filing Date
- 2018-07-23
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2038-07-23
AI Technical Summary
Existing isocyanate compositions used in coating films face issues with insufficient drying properties, viscosity stability, and solvent resistance, particularly when using triisocyanate compounds.
A specific isocyanate composition comprising a triisocyanate represented by general formula (I) and a compound represented by general formula (II), with a defined mass percentage of compound (II), is used to enhance viscosity stability and solvent resistance, where the triisocyanate can be lysine triisocyanate and the compound can be p-toluenesulfonyl isocyanate.
The isocyanate composition provides a coating composition with improved viscosity stability and solvent resistance, resulting in a coating film with better drying properties and reduced yellowing during storage.
Smart Images

Figure 0007590806000001 
Figure 0007590806000002 
Figure 0007590806000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an isocyanate composition, a coating composition, a coating, and a coated article. [Background technology]
[0002] Conventionally, urethane coating films formed from polyurethane paints have excellent flexibility, chemical resistance, and stain resistance. In particular, coating films using non-yellowing polyisocyanates obtained from aliphatic diisocyanates, such as hexamethylene diisocyanate (hereinafter sometimes referred to as "HDI"), as a curing agent, have excellent weather resistance, and the demand for them is increasing.
[0003] In recent years, with the growing concern for global environmental protection, technological developments have been actively carried out to reduce the viscosity of polyisocyanate compositions used as curing agents and to enable the reduction of organic solvents in paints. Examples of such methods include a method of using a low-viscosity triisocyanate compound alone (see, for example, Patent Documents 1 to 3, etc.). When these triisocyanate compounds are used, it is possible to achieve a low viscosity polyisocyanate composition. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 63-015264 [Patent Document 2] Japanese Patent Application Publication No. 53-135931 [Patent Document 3] Japanese Patent Publication No. 60-044561 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the triisocyanate compound described in Patent Document 1 is used, there is a problem that the drying property of the coating film is insufficient. Furthermore, when the triisocyanate compounds described in Patent Documents 2 and 3 were used, the drying properties of the coating film were satisfactory to a certain extent. However, there were problems such as the lack of viscosity stability of the coating composition, and the insufficient appearance, solvent resistance, and weather resistance of the resulting coating film.
[0006] The present invention has been made in view of the above circumstances, and provides an isocyanate composition that can give a coating composition having good viscosity stability and a coating film having good drying properties and solvent resistance. The present invention also provides a coating composition, a coating film, and a coated article using the isocyanate composition. [Means for solving the problem]
[0007] That is, the present invention includes the following aspects. The isocyanate composition according to the first aspect of the present invention contains a triisocyanate represented by the following general formula (I) and a compound represented by the following general formula (II), The content of the compound represented by the general formula (II) relative to the mass of the triisocyanate represented by the general formula (I) is 0.50 mass% or more and 5.00 mass% or less. .
[0008] [ka]
[0009] [In the general formula (I), 1 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain one or more structures selected from the group consisting of an ester structure and an ether structure. 1 may be the same or different. 1 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms.]
[0010] [ka]
[0011] [In general formula (II), R 2 R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 3is an isocyanate group. The triisocyanate represented by the general formula (I) may be lysine triisocyanate. The compound represented by the general formula (II) may be p-toluenesulfonyl isocyanate. 。
[0012] A coating composition according to a second aspect of the present invention comprises the isocyanate composition according to the first aspect and a polyol.
[0013] A coating film according to a third aspect of the present invention is obtained by curing the coating composition according to the second aspect.
[0014] A coated article according to a fourth aspect of the present invention comprises the coating film according to the third aspect. Effect of the Invention
[0015] According to the above-mentioned aspect, it is possible to provide an isocyanate composition which can obtain a coating composition having good viscosity stability and a coating film having good drying properties and solvent resistance. It is also possible to provide a coating composition, a coating film, and a coated article using the isocyanate composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0017] In this specification, the term "triisocyanate" refers to a monomer compound having three isocyanate groups (-NCO) in one molecule. As used herein, "polyol" refers to a compound having two or more hydroxy groups (-OH).
[0018] In this specification, unless otherwise specified, "(meth)acrylic" includes methacrylic and acrylic, and "(meth)acrylate" includes methacrylate and acrylate.
[0019] <Isocyanate composition> The isocyanate composition according to one embodiment of the present invention contains a triisocyanate represented by the following general formula (I) (hereinafter, may be referred to as "triisocyanate compound (I)") and a compound represented by the following general formula (II) (hereinafter, may be referred to as "compound (II)").
[0020] [ka]
[0021] [In the general formula (I), 1 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain one or more structures selected from the group consisting of an ester structure and an ether structure. 1 may be the same or different. 1 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms.]
[0022] [ka]
[0023] [In general formula (II), R 2 R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 3 is a halogen atom or an isocyanate group.
[0024] The isocyanate composition of the present embodiment provides a coating composition having good viscosity stability, and the isocyanate composition of the present embodiment provides a coating film having good drying properties and solvent resistance. The physical properties and constituent components of the isocyanate composition of the present embodiment will be described in detail below.
[0025] <Physical Properties> [Yellowing degree] It is preferable that the isocyanate composition of the present embodiment hardly yellows even when stored for a long period of time. Specifically, when the isocyanate composition of the present embodiment is stored at 60°C for one week, the upper limit of the Hazen color number (APHA) is preferably less than 100, more preferably less than 50, even more preferably less than 30, and particularly preferably less than 10. On the other hand, the lower limit of the Hazen color number (APHA) in the isocyanate composition of the present embodiment is not particularly limited, but may be, for example, 0 or more. When the Hazen color number of the isocyanate composition of the present embodiment is within the above range, it can be determined that the degree of yellowing during storage is small. The Hazen color index can be measured by a Hazen color index test using an ultraviolet-visible spectrophotometer as specified in ISO 6271-2:2004.
[0026] [viscosity] The viscosity of the isocyanate composition of the present embodiment at 25° C. is not particularly limited, but is preferably from 1 mPa·s to 1000 mPa·s, more preferably from 2 mPa·s to 500 mPa·s, and even more preferably from 5 mPa·s to 100 mPa·s. When the viscosity at 25° C. is equal to or greater than the above lower limit, curability tends to be better, and when the viscosity at 25° C. is equal to or less than the above upper limit, workability tends to be better. The viscosity can be measured by using an E-type viscometer (manufactured by Tokimec Co., Ltd.).
[0027] <Components> [Triisocyanate compound (I)] The triisocyanate compound (I) contained in the isocyanate composition of the present embodiment is represented by the above general formula (I).
[0028] (Y 1 ) In the general formula (I), 1 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain one or more structures selected from the group consisting of an ester structure and an ether structure. 1 may be the same or different.
[0029] The divalent hydrocarbon group having 1 to 20 carbon atoms may be an aliphatic group or an aromatic group. The aliphatic group may be linear, branched or cyclic. Examples of the linear or branched aliphatic group include an alkanediyl group (alkylene group), an alkylidene group, and the like. Examples of the cyclic aliphatic group include a cycloalkylene group. The aromatic group may, for example, be an arylene group such as a phenylene group. Among these, the divalent hydrocarbon group having 1 to 20 carbon atoms is preferably an alkylene group. Examples of the alkylene group include a methylene group, a dimethylene group, a trimethylene group, and a tetramethylene group. Among these, the alkylene group is preferably a tetramethylene group.
[0030] Also, Y 1 Examples of the divalent hydrocarbon group having 1 to 20 carbon atoms which may contain one or more selected from the group consisting of the ester structure and the ether structure in the above formula (III) include a group represented by the following formula (III) (hereinafter, sometimes referred to as "group (III)"). -(CH2) n1 -X-(CH2) n2 - (III)
[0031] In the group (III), -(CH2) n1 The bond opposite to X in - is bonded to C in the above general formula (I), and -(CH2) n2The bond opposite to the -X is bonded to NCO in the above general formula (I). Also, n1+n2 are integers satisfying 1≦n1+n2≦20. In other words, both n1 and n2 are not 0, and it is preferable that n2, which is bonded to NCO, is 1 or more. Among these, n1 and n2 are each independently preferably an integer of 0 to 20, more preferably an integer of 0 to 4, and further preferably an integer of 0 to 2. As the combination of n1 and n2, for example, the combination of n1=0, n2=2 and the combination of n1=2, n2=2 are preferable.
[0032] In the group (III), X is an ester structure or an ether structure. Among these, X is preferably an ester structure because the reaction rate increases.
[0033] Also, there are multiple Y 1 When at least one of the isocyanate composition of the present embodiment has one or more types selected from the group consisting of an aliphatic group and an aromatic group, the viscosity of the isocyanate composition of the present embodiment can be made lower, and the weather resistance of a coating film produced by using the isocyanate composition of the present embodiment as a curing agent for a coating composition can be made better. Also, there are multiple Y 1 When at least one of them has an ester structure, the heat resistance of the isocyanate composition of the present embodiment can be further improved, and the curing property of a coating film produced by using the isocyanate composition of the present embodiment as a curing agent for a coating composition can be further improved.
[0034] (R 1 ) R 1 R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 1 The hydrocarbon group in is not particularly limited, and examples thereof include an alkyl group, an alkenyl group, and an alkynyl group. 1 is preferably a hydrogen atom.
[0035] In the present embodiment, specific examples of preferred triisocyanate compounds (I) include bis(2-isocyanatoethyl)2-isocyanatoglutarate (hereinafter referred to as "GTI", molecular weight 311) disclosed in JP-B-4-1033 (Reference 1), lysine triisocyanate (hereinafter referred to as "LTI", molecular weight 267) disclosed in JP-A-53-135931 (Reference 2), and 4-isocyanatomethyl-1,8-octamethylene diisocyanate (hereinafter referred to as "NTI", molecular weight 251) disclosed in WO 1996 / 17881 (Reference 3).
[0036] Among these, as the triisocyanate compound (I), LTI is preferred since it has a higher reactivity of the isocyanate group and can further improve the compatibility with polar solvents.
[0037] (Molecular weight of triisocyanate compound) The molecular weight of the triisocyanate compound (I) contained in the isocyanate composition of the present embodiment is preferably 139 or more and 1,000 or less, more preferably 150 or more and 800 or less, even more preferably 180 or more and 600 or less, and particularly preferably 200 or more and 400 or less. When the molecular weight of the triisocyanate compound (I) is equal to or more than the above lower limit, crystallization can be further suppressed, and when it is equal to or less than the above upper limit, a low viscosity can be more easily achieved.
[0038] [Method for producing triisocyanate compound (I)] The triisocyanate compound (I) contained in the isocyanate composition of the present embodiment can be obtained, for example, by isocyanating an amine such as an amino acid derivative or an ether amine.
[0039] Examples of the amino acid derivatives include 2,5-diaminovaleric acid, 2,6-diaminohexanoic acid, aspartic acid, and glutamic acid. These amino acid derivatives are diamine monocarboxylic acids or monoamine dicarboxylic acids. Therefore, the number of amino groups can be controlled by esterifying the carboxyl group with an alkanolamine such as ethanolamine. Alternatively, the number of amino groups can be controlled by esterifying the carboxyl group with an alcohol such as methanol. The obtained amine having an ester group can be converted into a triisocyanate compound containing an ester structure by, for example, phosgenating the amine.
[0040] An example of the etheramine is polyoxyalkylene triamine under the trade name "D403" of Mitsui Fine Chemicals, Inc. These etheramines are triamines, and can be converted into triisocyanate compounds containing an ether structure by phosgenation of the amine, or the like.
[0041] [Compound (II)] The compound (II) contained in the isocyanate composition of the present embodiment is represented by the above general formula (II).
[0042] (R 2 ) R 2 R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 2 The hydrocarbon group in is not particularly limited, and examples thereof include an alkyl group, an alkenyl group, and an alkynyl group. The alkyl group, the alkenyl group, and the alkynyl group may be linear, branched, or cyclic (aliphatic cyclic group). The number of carbon atoms in these groups is preferably 1 to 12, more preferably 1 to 6, and further preferably 1 to 3. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group (a tert-butyl group), a pentyl group, an isoamyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. Examples of the alkenyl group include a vinyl group, an allyl group, a 1-propenyl group, an isopropenyl group, a 2-butenyl group, a 1,3-butadienyl group, a 2-pentenyl group, and a 2-hexenyl group. Examples of the alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl group, an isopropynyl group, a 1-butynyl group, and an isobutynyl group. Among them, R 2 As the alkyl group, a methyl group is preferable.
[0043] (R 3 ) R 3 is a halogen atom or an isocyanate group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Among them, R 3 As the alkyl group, an isocyanate group is preferable.
[0044] In the present embodiment, specific examples of preferred compound (II) include p-toluenesulfonyl isocyanate, p-toluenesulfonyl chloride, and p-toluenesulfonyl bromide.
[0045] Among these, p-toluenesulfonyl isocyanate is preferred as compound (II) since no toxic gas is generated during storage of the isocyanate composition of this embodiment, during production of the coating composition, and during formation of a coating film.
[0046] (Content of Compound (II)) The content of compound (II) in the isocyanate composition of the present embodiment is preferably 0.01 mass% or more and less than 10 mass%, more preferably 0.1 mass% or more and less than 7 mass%, and even more preferably 0.2 mass% or more and less than 3 mass%, relative to the mass of isocyanate compound (I). By the content of the compound (II) contained in the isocyanate composition of this embodiment being equal to or greater than the lower limit, the viscosity stability of the coating composition containing the isocyanate composition of this embodiment, and the appearance (sharpness) and solvent resistance of the coating film obtained tend to be more excellent. On the other hand, by the content of the compound (II) contained in the isocyanate composition of this embodiment being less than the upper limit, the yellowing resistance of the coating composition containing the isocyanate composition of this embodiment during storage, and the appearance (sharpness), solvent resistance, and gloss retention rate (weather resistance) of the coating film obtained when irradiated with ultraviolet light tend to be more excellent.
[0047] [Method for producing compound (II)] The compound (II) contained in the isocyanate composition of the present embodiment is, for example, an aromatic compound such as toluene, a halogenated sulfonic acid, chlorosulfonyl isocyanate, or the like, which is one of the above-mentioned R 3 It can be obtained by reacting a compound having a group and a sulfonyl group (see reaction formula (1) below). In addition, X' in reaction formula (1) is a halogen atom or a hydroxyl group. R 2 C6H5+X'SO2R 3 → pR 2 C6H4SO2R 3 + HX' (1)
[0048] Specifically, for example, p-toluenesulfonyl isocyanate can be obtained by reacting toluene with chlorosulfonyl isocyanate (see the following reaction formula (2)). CH3C6H5+ClSO2NCO → p-CH3C6H4SO2NCO + HCl ···(2)
[0049] [Other isocyanate compounds] The isocyanate composition of the present embodiment may further contain a different isocyanate compound in addition to the above-mentioned triisocyanate compound (I) and the above-mentioned compound (II). Examples of the different isocyanate compounds include diisocyanates having two aliphatic, alicyclic, or aromatic isocyanate groups, etc. Alternatively, the compound may be a polyisocyanate, which is a reaction product obtained by reacting an isocyanate compound having one or more aliphatic, alicyclic, or aromatic isocyanate groups using a catalyst or by heating the compound.
[0050] Examples of the diisocyanate include tetramethylene diisocyanate (TMDI), pentamethylene diisocyanate (PDI), hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexane-1,6-diisocyanate, 2-methylpentane-1,5-diisocyanate (MPDI), 1,3-bis(isocyanatomethyl)-cyclohexane (1,3-H6-XDI), 3(4)-isocyanate, and the like. Examples of the diisocyanates include 1-methyl-1,2-dimethyl-2,4-dimethylphenyl diisocyanate (DMDI), 1,3-bis(isocyanatomethyl)-benzene, 1,3-bis(2-isocyanatopropyl-2)benzene, 4,4'-dicyclohexylmethane diisocyanate (H12MDI), lysine diisocyanate (LDI), etc. These diisocyanates may be used alone or in combination of two or more. Among these, the diisocyanate is preferably HDI or IPDI in view of the weather resistance of the resulting coating film and ease of industrial availability.
[0051] The polyisocyanate is preferably a reaction product obtained by reacting the above-mentioned diisocyanate. The polyisocyanate molecule contains, for example, an isocyanurate group, a uretdione group, an allophanate group, an iminooxadiazinedione group, a urethane group, a biuret group, and the like. Among these, the polyisocyanate is preferably one containing an isocyanurate group from the viewpoint of weather resistance.
[0052] ≪Paint composition≫ A coating composition according to one embodiment of the present invention contains the above-mentioned isocyanate composition and a polyol.
[0053] The coating composition of the present embodiment contains the above-mentioned isocyanate composition, and therefore has good viscosity stability over time. Furthermore, the coating composition of the present embodiment can provide a coating film with good drying properties and solvent resistance. The physical properties and constituent components of the coating composition of this embodiment will be described in detail below.
[0054] <Physical Properties> [Viscosity increase rate] The coating composition of the present embodiment exhibits little change in viscosity over time and is stable. Specifically, the upper limit of the viscosity increase rate of the coating composition of this embodiment is preferably less than 2.0, more preferably less than 1.5, and even more preferably less than 1.3. On the other hand, the lower limit of the viscosity increase rate of the coating composition of this embodiment is not particularly limited, but may be, for example, 1.0 or more. When the viscosity increase rate of the coating composition of this embodiment is within the above range, it can be determined that the viscosity increase rate is stable. The viscosity increase rate can be calculated from the ratio of the viscosity (B) at 25° C. 3 hours after production to the viscosity (A) at 25° C. immediately after production (see formula (a) below). Paint viscosity increase rate = Viscosity 3 hours after production (B) / Viscosity immediately after production (A) (a) The viscosity at 25° C. can be measured using an E-type viscometer (manufactured by Tokimec Co., Ltd.).
[0055] <Components> The isocyanate composition contained in the coating composition of the present embodiment is as described above. The coating composition of the present embodiment also contains a polyol as a resin component. The polyol is a compound having two or more active hydrogens in the molecule, and is reactive with the isocyanate group of the above-mentioned isocyanate composition. Examples of compounds having two or more active hydrogens in the molecule other than polyols include polyamines and polythiols. Among these, polyols are preferred as the compound having two or more active hydrogens in the molecule contained in the coating composition of this embodiment.
[0056] [Polyol] Examples of the polyol include polyester polyol, polyether polyol, acrylic polyol, polyolefin polyol, and fluorine polyol. Among them, the polyol is preferably an acrylic polyol from the viewpoint of the weather resistance, solvent resistance, and hardness of the resulting coating film, or a polyester polyol from the viewpoint of the mechanical strength and oil resistance of the resulting coating film.
[0057] (Polyester polyol) The polyester polyol can be obtained, for example, by subjecting a dibasic acid, or a mixture of two or more kinds, and a polyhydric alcohol, or a mixture of two or more kinds, to a condensation reaction. Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.
[0058] As a specific method for producing the polyester polyol, for example, the above components are mixed and heated at about 160°C to 220°C to carry out a condensation reaction. Alternatively, for example, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone with polyhydric alcohols can also be used as polyester polyols. These polyester polyols can be modified with aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, and polyisocyanates obtained from these. In particular, from the viewpoint of the yellowing resistance of the coating composition of the present embodiment and the weather resistance of the resulting coating film, it is preferable to modify the polyester polyol with an aliphatic diisocyanate, an alicyclic diisocyanate, or a polyisocyanate obtained from these.
[0059] Furthermore, when the coating composition of this embodiment is used as an aqueous base coating, a portion of the carboxylic acid derived from the dibasic acid or the like in the polyester polyol can be left to remain and neutralized with a base such as an amine or ammonia, thereby converting the polyester polyol into a water-soluble or water-dispersible resin.
[0060] (Polyether polyol) The polyether polyol can be obtained, for example, by using any one of the following methods (1) to (3). (1) A method in which an alkylene oxide or a mixture thereof is randomly or block-added to a polyhydric hydroxy compound or a mixture thereof using a catalyst to obtain polyether polyols. (2) A method in which a polyamine compound is reacted with an alkylene oxide to obtain a polyether polyol. (3) A method in which the polyether polyols obtained by (1) or (2) are used as a medium to polymerize acrylamide or the like to obtain so-called polymer polyols.
[0061] Examples of the catalyst include hydroxides (lithium, sodium, potassium, etc.), strong basic catalysts (alcoholates, alkylamines, etc.), composite metal cyanide complexes (metal porphyrins, zinc hexacyanocobaltate complexes, etc.), and the like.
[0062] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.
[0063] Examples of the polyhydric hydroxy compound include the following. (i) Diglycerin, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc. (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabinitol, ribitol, xylitol, sorbitol, mannitol, galactitol, and rhamnitol. (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbose, rhamnose, fucose, and ribosaccharides. (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose, and melibiose. (v) Trisaccharides such as raffinose, gentianose, and melezitose. (vi) Tetrasaccharides such as stachyose.
[0064] Examples of the polyamine compound include ethylenediamines.
[0065] (Acrylic polyol) The acrylic polyol can be obtained, for example, by polymerizing a polymerizable monomer having one or more active hydrogens in one molecule, or by copolymerizing a polymerizable monomer having one or more active hydrogens in one molecule with another monomer copolymerizable with the polymerizable monomer, as necessary.
[0066] Examples of the polymerizable monomer having one or more active hydrogens in one molecule include the following. These may be used alone or in combination of two or more kinds. (i) Acrylic esters having active hydrogen, such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-hydroxybutyl acrylate. (ii) Methacrylic acid esters having active hydrogen, such as 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate. (iii) (meth)acrylic acid esters having polyvalent active hydrogen, such as (meth)acrylic acid monoesters of triols such as glycerin and trimethylolpropane. (iv) Monoethers of polyether polyols (for example, polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.) and the above-mentioned (meth)acrylic acid esters having active hydrogen. (v) Adducts of glycidyl (meth)acrylate with monobasic acids (eg, acetic acid, propionic acid, p-tert-butylbenzoic acid, etc.). (vi) Adducts obtained by ring-opening polymerization of lactones (for example, ε-caprolactam, γ-valerolactone, etc.) with the active hydrogen of the above-mentioned (meth)acrylic acid esters having active hydrogen.
[0067] Examples of other monomers copolymerizable with the polymerizable monomer include the following. These may be used alone or in combination of two or more. (i) (Meth)acrylic acid esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate, and glycidyl methacrylate. (ii) Unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid. (iii) Unsaturated amides such as acrylamide, N-methylol acrylamide, and diacetone acrylamide. (iv) Vinyl monomers having a hydrolyzable silyl group, such as vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane. (v) Other polymerizable monomers such as styrene, vinyl toluene, vinyl acetate, acrylonitrile, dibutyl fumarate, etc.
[0068] A specific example of a method for producing the acrylic polyol is a method in which the above-mentioned monomer components are solution polymerized in the presence of a radical polymerization initiator such as a known peroxide or an azo compound, and the resulting solution is diluted with an organic solvent, etc., as necessary, to obtain the acrylic polyol.
[0069] When the coating composition of the present embodiment is used as a water-based coating, a water-based acrylic polyol can be produced by using a known method such as a method of solution-polymerizing the above-mentioned monomer components and converting them into a water layer, or emulsion polymerization. In this case, the acidic portion of the carboxylic acid-containing monomer such as acrylic acid or methacrylic acid or the sulfonic acid-containing monomer can be neutralized with an amine or ammonia to impart water solubility or water dispersibility to the acrylic polyol.
[0070] (Polyolefin polyol) Examples of the polyolefin polyol include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene having two or more hydroxyl groups, polyisoprene having two or more hydroxyl groups, and hydrogenated polyisoprene having two or more hydroxyl groups. In addition, in the polyolefin polyol, the number of hydroxyl groups is preferably 3, since higher coating strength can be obtained.
[0071] (Fluoropolyol) In this specification, the term "fluorine polyol" refers to a polyol containing fluorine in the molecule. Specific examples of the fluorine polyol include copolymers of fluoroolefin, cyclovinyl ether, hydroxyalkyl vinyl ether, monocarboxylic acid vinyl ester, etc., as disclosed in JP-A-57-34107 (Reference 4) and JP-A-61-275311 (Reference 5).
[0072] (Hydroxyl value and acid value of polyol) The hydroxyl value of the polyol is not particularly limited, but is preferably from 10 mgKOH / g to 200 mgKOH / g, more preferably from 20 mgKOH / g to 200 mgKOH / g, and even more preferably from 30 mgKOH / g to 200 mgKOH / g. The acid value of the polyol is preferably from 0 mgKOH / g to 30 mgKOH / g. The hydroxyl value and acid value can be measured in accordance with JIS K1557.
[0073] (NCO / OH) The molar equivalent ratio (NCO / OH) of the isocyanate group of the isocyanate composition to the hydroxyl group of the polyol is preferably 0.2 to 5.0, more preferably 0.4 to 3.0, and even more preferably 0.5 to 2.0. When the molar equivalent ratio is equal to or greater than the lower limit, a tougher coating film can be obtained. When the molar equivalent ratio is equal to or less than the upper limit, the smoothness of the coating film obtained can be further improved.
[0074] [Other additives] In addition to the above-mentioned isocyanate composition and polyol, the coating composition of the present embodiment may further contain various additives used in the relevant technical field, such as organic solvents, catalysts for curing promotion, pigments, leveling agents, antioxidants, ultraviolet absorbers, light stabilizers, plasticizers, and surfactants, depending on the purpose and application, within a range that does not impair the effects of the present embodiment.
[0075] (Organic solvent) The organic solvent is preferably one that does not have a functional group that reacts with a hydroxyl group or an isocyanate group, and is preferably one that is compatible with the above-mentioned isocyanate composition. Specific examples of the organic solvent include organic solvents that are generally used as paint solvents, such as ester compounds, ether compounds, ketone compounds, aromatic compounds, ethylene glycol dialkyl ether compounds, polyethylene glycol dicarboxylate compounds, hydrocarbon solvents, and aromatic solvents.
[0076] (Catalyst for accelerating curing) Examples of catalysts for promoting curing include metal salts such as dibutyltin dilaurate, tin 2-ethylhexanoate, zinc 2-ethylhexanoate, and cobalt salts; and tertiary amines such as triethylamine, pyridine, methylpyridine, benzyldimethylamine, N,N-dimethylcyclohexylamine, N-methylpiperidine, pentamethyldiethylenetriamine, N,N'-endoethylenepiperazine, and N,N'-dimethylpiperazine.
[0077] <Method of producing coating composition> The coating composition of the present embodiment may be used as a solvent-based coating composition or as a water-based coating composition. When the coating composition of the present embodiment is used as a solvent-based coating, it can be produced by the following method. First, to the polyol or its solvent dilution, additives such as other resins, catalysts for curing promotion, pigments, leveling agents, antioxidants, UV absorbers, light stabilizers, plasticizers, surfactants, etc. are added as necessary. Then, the above-mentioned isocyanate composition is added as a curing agent, and if necessary, a solvent is further added to adjust the viscosity. Then, the mixture is stirred by hand or with a stirring device such as a mixer to obtain a solvent-based paint.
[0078] When the coating composition of the present embodiment is used as a water-based base coating, it can be produced by the following method. First, to the aqueous dispersion or aqueous solution of the resin containing polyol, additives such as other resins, catalysts for curing promotion, pigments, leveling agents, antioxidants, UV absorbers, light stabilizers, plasticizers, surfactants, etc. are added as necessary. Then, the above-mentioned isocyanate composition is added as a curing agent, and if necessary, water or a solvent is further added to adjust the viscosity. Then, the mixture is forcedly stirred with a stirring device such as a mixer to obtain a water-based base paint.
[0079] <Application> The coating composition of the present embodiment can be used as a coating material for roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, and the like. The coating composition of the present embodiment is also useful as a primer or topcoat for materials such as metals (steel plates, surface-treated steel plates, etc.), plastics, wood, films, and inorganic materials. The coating composition of the present embodiment is also useful as a coating for imparting cosmetic properties, weather resistance, acid resistance, rust resistance, chipping resistance, etc. to pre-coated metals including rust-resistant steel plates, painted parts of automobiles, etc. The coating composition of the present embodiment is also useful as a urethane raw material for adhesives, pressure sensitive adhesives, elastomers, foams, surface treatment agents, and the like.
[0080] <Coating film> A coating film according to one embodiment of the present invention is obtained by curing the above-mentioned coating composition.
[0081] The coating film of the present embodiment is obtained by applying the above-mentioned coating composition using a known method such as roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, etc., and then drying or baking at room temperature to harden the coating film. The coating film of this embodiment has good drying properties and solvent resistance.
[0082] <Painted items> A coated article according to one embodiment of the present invention comprises the above-mentioned coating film.
[0083] The coated article of this embodiment can be obtained by applying the above-mentioned coating composition to the surface of any article using a known method such as roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, etc., and then drying or baking the composition at room temperature to harden the composition to form a coating film on the surface of the article. The coated article of this embodiment has the above-mentioned coating film that has good drying properties and solvent resistance, and is endowed with cosmetic properties, acid resistance, rust prevention, chipping resistance, adhesion, and the like. EXAMPLES
[0084] Hereinafter, the present embodiment will be described in more detail with reference to specific examples and comparative examples. However, the present embodiment is not limited in any way to the following examples and comparative examples as long as the gist of the present embodiment is not exceeded. In the following, Examples 1, 5, 6, 7, 11, and 12 are considered as reference examples.
[0085] <Test items> According to the methods described below, the isocyanate compositions produced in the examples and comparative examples, the coating compositions containing the isocyanate compositions, and the coating films obtained from the coating compositions were subjected to measurement and evaluation of the physical properties described below.
[0086] <Physical property 1: NCO content> The NCO content (mass %) was determined by neutralizing the isocyanate groups in each isocyanate composition with an excess of 2N amine and then back titrating with 1N hydrochloric acid.
[0087] <Evaluation of isocyanate composition 1: Yellowing of isocyanate composition during storage> The isocyanate composition was stored at 60°C for one week. The sample after storage was filtered through a membrane filter with a pore size of 3 μm. The filtered sample was then placed in a cell with a length of 5 cm, and the Hazen color number (APHA) was measured in an environment of 25°C using a measuring device Lovibond PFXi-195. From the measurement results, yellowing during storage was evaluated according to the following evaluation criteria. (Evaluation Criteria) ◎: Less than 10 ○: 10 or more, less than 30 △: 30 or more, less than 50 ×:50 or more
[0088] <Paint composition evaluation 1: Paint viscosity increase rate> The viscosity (A) immediately after production and the viscosity (B) 3 hours after production of each coating composition produced in the Examples and Comparative Examples were measured at 25°C using an E-type viscometer (Tokimec Co., Ltd.) For the measurements, a standard rotor (1°34' x R24) was used, and the rotation speeds were as follows: 100 rpm (less than 128 mPa s) 50 rpm (for 128 mPa s or more and less than 256 mPa s) 20 rpm (256 mPa s or more but less than 640 mPa s) 10 rpm (for values between 640 mPa s and 1280 mPa s) 5 rpm (for 1280 mPa s or more but less than 2560 mPa s)
[0089] Next, the paint viscosity increase rate was calculated from the measured viscosity (A) immediately after production and the viscosity (B) 3 hours after production according to the following formula (a). Paint viscosity increase rate = Viscosity 3 hours after production (B) / Viscosity immediately after production (A) (a)
[0090] The calculated viscosity increase rate of the coating composition was evaluated according to the following evaluation criteria. (Evaluation Criteria) ◎: 1.0 or more and less than 1.3 ○: 1.3 or more and less than 1.5 △: 1.5 or more and less than 2.0 ×: 2.0 or higher
[0091] <Evaluation of coating film 1: Drying property of coating film (gel fraction)> About 0.1 g of each coating film produced in the examples and comparative examples was precisely weighed. Then, about 0.1 g of each coating film was put into 10 g of acetone and shaken at 23°C for 1 hour. Then, the acetone solution containing each coating film after shaking was filtered through a 325 mesh metal mesh. Then, the insoluble portion of the coating film remaining on the mesh was dried in a hot air dryer at 120°C for 1 hour, and the dry weight was precisely weighed. Then, the dry weight of the acetone insoluble portion was divided by the original weight of 0.1 g to calculate the gel fraction. The calculated gel fraction was evaluated for coating drying property according to the following evaluation criteria. (Evaluation Criteria) ◎: 95% or more ○: 90% or more but less than 95% △: 85% to less than 90% ×: Less than 85%
[0092] <Coating film evaluation 2: Coating film appearance (sharpness)> When a fluorescent lamp was applied to each of the coating films produced in the Examples and Comparative Examples, the clarity of the fluorescent lamp reflected by the coating film was compared. Next, the coating film appearance (sharpness) was evaluated according to the following evaluation criteria. (Evaluation Criteria) Sharpness of the reflected image of fluorescent lamps (relative comparison): Good ◎>○>△>× Bad
[0093] <Paint film evaluation 3: Solvent resistance (xylene)> Cotton soaked in xylene was placed on each coating film produced in the Examples and Comparative Examples, and left for 5 minutes at 23°C. The cotton was then removed, the xylene on the coating film was wiped off, and the coating film surface was observed. The solvent resistance (xylene) was then evaluated according to the following evaluation criteria. (Evaluation Criteria) ◎: No traces of testing ○: There were slight traces of testing △: There were traces of testing ×: Traces of the test were found, and the coating film had deteriorated.
[0094] <Paint film evaluation 4: Weather resistance of paint film (QUV)> The coating films produced in the examples and comparative examples were subjected to a QUV test under the following conditions. (QUV test conditions) Equipment: Dewpanel light control weather meter (Model FDP, manufactured by Suga Test Instruments) Irradiance: 28W / m2 Cycle: 60℃×10%RH×4 hours → Dark: 50℃×95%RH×4 hours Test time: 1000 hours
[0095] The gloss retention rate was measured from the gloss values of the coating film before and after the test.Then, the weather resistance (QUV) of the coating film was evaluated according to the following evaluation criteria. (Evaluation Criteria) ◎: 95% or more ○: 90% or more but less than 95% △: 85% to less than 90% ×: Less than 85%
[0096] [Synthesis Example 1] Synthesis of LTI In a four-neck flask equipped with a stirrer, a thermometer, and a gas inlet tube, 122.2 g of ethanolamine, 100 mL of o-dichlorobenzene, and 420 mL of toluene were placed, and ice-cooled hydrogen chloride gas was introduced to convert the ethanolamine to hydrochloride. Then, 182.5 g of lysine hydrochloride was added, and the reaction solution was heated to 80° C. to dissolve the ethanolamine hydrochloride, and hydrogen chloride gas was introduced to convert it to lysine dihydrochloride. Then, hydrogen chloride gas was passed through at 20 to 30 mL / min, and the reaction solution was heated to 116° C., and this temperature was maintained until water was no longer distilled. The resulting reaction mixture was then recrystallized in a mixture of methanol and ethanol to obtain 165 g of lysine β-aminoethyl ester trihydrochloride. 100 g of this lysine β-aminoethyl ester trihydrochloride was suspended as fine powder in 1200 mL of o-dichlorobenzene, and the reaction solution was heated while stirring. Next, when the reaction solution reached 120°C, phosgene was started to be blown in at a rate of 0.4 mol / hour, and the temperature was maintained for 10 hours. Next, the reaction solution was heated to 150°C, and most of the lysine β-aminoethyl ester trihydrochloride in the reaction solution was dissolved. Next, after cooling, the solution was filtered, and the dissolved phosgene and the solvent were distilled off under reduced pressure. Next, 80.4 g of colorless and transparent LTI with a boiling point of 155 to 157°C / 0.022 mmHg was obtained by vacuum distillation. The NCO content of LTI was 47.1% by weight.
[0097] [Synthesis Example 2] Synthesis of NTI In a four-neck flask equipped with a stirrer, a thermometer, and a gas inlet tube, 1060 g of 4-aminomethyl-1,8-octamethylenediamine (hereinafter sometimes referred to as "triamine") was dissolved in 1500 g of methanol, and 1800 mL of 35% concentrated hydrochloric acid was gradually added dropwise to the solution while cooling. The solution was concentrated by removing methanol and water under reduced pressure, and dried at 60°C / 5 mmHg for 24 hours to obtain a white solid triamine hydrochloride. 650 g of the obtained triamine hydrochloride was suspended as a fine powder in 5000 g of o-dichlorobenzene, and the reaction solution was heated while stirring. When the temperature reached 100°C, phosgene was started to be blown in at a rate of 200 g / Hr, and the temperature was further increased to 180°C, and phosgene was continued to be blown in for 12 hours. The dissolved phosgene and the solvent were removed under reduced pressure, and then vacuum distillation was performed to obtain 420 g of colorless and transparent 4-isocyanatemethyl-1,8-octamethylene diisocyanate (hereinafter sometimes referred to as "NTI") having a boiling point of 161 to 163°C / 1.2 mmHg. The NCO content of NTI was 50.0% by weight.
[0098] [Examples 1 to 6] Production of isocyanate compositions PI-a1 to PI-a6, coating compositions C-a1 to C-a6, and coating films T-a1 to T-a6 (1) Production of Isocyanate Compositions PI-a1 to PI-a6 The content of p-toluenesulfonyl isocyanate (manufactured by Wako Pure Chemical Industries, Ltd.) relative to the mass of LTI obtained in Synthesis Example 1 was mixed to obtain the value shown in Table 1, thereby obtaining isocyanate compositions PI-a1 to PI-a6 (hereinafter sometimes simply referred to as "PI-a1" to "PI-a6"). The yellowing during storage of the obtained PI-a1 to PI-a6 was evaluated according to the above-mentioned evaluation method, and the results are shown in Table 1 below.
[0099] (2) Preparation of Coating Compositions C-a1 to C-a6 Next, PI-a1 to PI-a6 produced in (1) were allowed to stand at 23° C. for one month. Next, each isocyanate composition and acrylic polyol (Nuplex Resin's product name "SETALUX1753", resin concentration 70%, hydroxyl value 138.6 mgKOH / g) were mixed so that the equivalent ratio of isocyanate group / hydroxyl group was 1.1. Then, the solid content was adjusted to 60 mass% with butyl acetate to obtain coating compositions C-a1 to C-a6. The viscosity increase rates of the resulting coating compositions C-a1 to C-a6 were evaluated according to the above-mentioned evaluation method, and the results are shown in Table 1 below.
[0100] (3) Manufacture of coating films T-a1 to T-a6 Next, each coating composition obtained in (2) was left to stand at 23°C / 50%RH for 3 hours. Next, each coating composition was applied onto a glass plate so that the dry film thickness was 60 μm. Next, the coating composition was cured by treating for 60 minutes at 23°C / 50%RH and for 1 hour in a hot air dryer at 120°C to obtain coating films 1 to 6. The drying property (gel fraction), appearance (sharpness) and weather resistance of the obtained coating films Ta1 to Ta6 were evaluated according to the above-mentioned evaluation methods. The results are shown in Table 1 below.
[0101] Comparative Examples 1-2: Production of Isocyanate Composition PI-b1, Coating Compositions C-b1-C-b2, and Coating Films T-b1-T-b2 (1) Preparation of isocyanate composition PI-b1 The LTI obtained in Synthesis Example 1 was mixed so that the mass of the LTI was the value shown in Table 2, to obtain an isocyanate composition PI-b1 (hereinafter, sometimes simply referred to as "PI-b1"). The yellowing of the obtained PI-b1 during storage was evaluated according to the above-mentioned evaluation method, and the results are shown in Table 2 below.
[0102] (2) Production of Coating Compositions C-b1 to C-b2 Next, PI-b1 produced in (1) was left to stand at 23°C for one month. Next, the isocyanate composition PI-b1 and acrylic polyol (product name "SETALUX1753" of Nuplex Resin Co., Ltd., resin content concentration 70%, hydroxyl value 138.6mgKOH / g) were mixed so that the equivalent ratio of isocyanate group / hydroxyl group was 1.1. Furthermore, 0.17 parts by mass of p-toluenesulfonyl isocyanate was mixed for coating composition C-b2. Next, the solid content was adjusted to 60% by mass with butyl acetate to obtain coating compositions C-b1 to C-b2. The viscosity increase rates of the resulting coating compositions C-b1 and C-b2 were evaluated according to the above-mentioned evaluation method, and the results are shown in Table 2 below.
[0103] (3) Production of coating films T-b1 to T-b2 Next, coating films T-b1 to T-b2 were obtained in the same manner as in (3) of Examples 1 to 6 using each of the coating compositions obtained in (2). The drying property (gel fraction), appearance (sharpness) and weather resistance of the obtained coating films T-b1 to T-b2 were evaluated according to the above-mentioned evaluation methods. The results are shown in Table 2 below.
[0104] [Examples 7 to 12] Production of isocyanate compositions PI-a7 to PI-a12, coating compositions C-a7 to C-a12, and coating films T-a7 to T-a12 (1) Production of Isocyanate Compositions PI-a7 to PI-a12 The NTI obtained in Synthesis Example 2 was mixed with p-toluenesulfonyl isocyanate (manufactured by Wako Pure Chemical Industries, Ltd.) so that the content thereof relative to the mass thereof was the value shown in Table 3, thereby obtaining isocyanate compositions PI-a7 to PI-a12. The yellowing during storage of the obtained PI-a7 to PI-a12 was evaluated according to the above-mentioned evaluation method, and the results are shown in Table 3 below.
[0105] (2) Preparation of Coating Compositions C-a7 to C-a12 Next, coating compositions C-a7 to C-a12 were obtained in the same manner as in (2) of Examples 1 to 6, except that PI-a7 to PI-a12 produced in (1) were used. The viscosity increase rates of the resulting coating compositions C-a7 to C-a12 were evaluated according to the above-mentioned evaluation method, and the results are shown in Table 3 below.
[0106] (3) Manufacture of coating films T-a7 to T-a12 Next, coating films Ta7 to Ta12 were obtained in the same manner as in (3) of Examples 1 to 6 using each of the coating compositions obtained in (2). The drying property (gel fraction), appearance (sharpness) and weather resistance of the obtained coating films Ta7 to Ta12 were evaluated according to the above-mentioned evaluation methods. The results are shown in Table 3 below.
[0107] [Comparative Examples 3-4] Production of isocyanate composition PI-b3, coating compositions C-b3 to C-b4, and coating films T-b3 to T-b4 (1) Preparation of isocyanate composition PI-b3 The LTI obtained in Synthesis Example 1 was mixed so that the mass thereof became the value shown in Table 4, to obtain an isocyanate composition PI-b3 (hereinafter, sometimes simply referred to as "PI-b3"). The yellowing of the obtained PI-b3 during storage was evaluated according to the above-mentioned evaluation method, and the results are shown in Table 4 below.
[0108] (2) Production of Coating Compositions C-b3 to C-b4 Next, PI-b3 produced in (1) was left to stand at 23°C for one month. Next, the isocyanate composition PI-b3 and an acrylic polyol (Nuplex Resin's product name "SETALUX1753", resin content concentration 70%, hydroxyl value 138.6mgKOH / g) were mixed so that the equivalent ratio of isocyanate group / hydroxyl group was 1.1. Furthermore, for the coating composition C-b4, 0.17 parts by mass of p-toluenesulfonyl isocyanate was mixed. Next, the solid content was adjusted to 60% by mass with butyl acetate to obtain coating compositions C-b3 to C-b4. The viscosity increase rates of the resulting coating compositions C-b3 to C-b4 were evaluated according to the above-mentioned evaluation method, and the results are shown in Table 4 below.
[0109] (3) Production of coating films T-b3 to T-b4 Next, coating films T-b3 to T-b4 were obtained in the same manner as in (3) of Examples 1 to 6 using each of the coating compositions obtained in (2). The drying property (gel fraction), appearance (sharpness) and weather resistance of the obtained coating films T-b3 to T-b4 were evaluated according to the above-mentioned evaluation methods. The results are shown in Table 4 below.
[0110] [Table 1]
[0111] [Table 2]
[0112] [Table 3]
[0113] [Table 4]
[0114] From Examples 1 to 12, the coating compositions C-a1 to C-a12 containing the isocyanate compositions PI-a1 to PI-a12 containing LTI or NTI as the triisocyanate and p-toluenesulfonyl isocyanate had a viscosity increase rate of less than 2.0 and good viscosity stability. Furthermore, the coating films Ta1 to Ta12 obtained by curing the coating compositions Ca1 to Ca12 had good drying properties and solvent resistance. Moreover, the isocyanate compositions PI-a1 to PI-a5 and PI-a7 to PI-a11 had an APHA of less than 50 and showed particularly low yellowing during storage. Furthermore, the coating films T-a1 to T-a5 and T-a7 to T-a12 obtained by curing the coating compositions C-a1 to C-a5 and C-a7 to C-a12 containing the isocyanate compositions PI-a1 to PI-a5 and PI-a7 to PI-a12 respectively, also had particularly good appearances. Furthermore, the coating films T-a1 to T-a5 and T-a7 to T-a11 obtained by curing the coating compositions C-a1 to C-a5 and C-a7 to C-a11 containing the isocyanate compositions PI-a1 to PI-a5 and PI-a7 to PI-a11 respectively, were also particularly good in terms of weather resistance.
[0115] On the other hand, in Comparative Examples 1 to 4, the isocyanate compositions PI-b1 and PI-b3 composed only of triisocyanate had an APHA of less than 50 and showed little yellowing during storage. However, the coating compositions C-b1 and C-b3 containing the isocyanate compositions PI-b1 and PI-b3 had a viscosity increase rate of 2.0 or more and were poor in viscosity stability. In addition, the paint compositions C-b2 and C-b4, which contained the isocyanate compositions PI-b1 and PI-b3 and to which p-toluenesulfonyl isocyanate was added later, also had a viscosity increase rate of 2.0 or more and had poor viscosity stability. Furthermore, the coating films T-b1 and T-b2 obtained by curing the coating compositions C-b1 and C-b2 had good drying properties and weather resistance, but were poor in appearance and solvent resistance. Furthermore, the coating films T-b3 and T-b4 obtained by curing the coating compositions C-b3 and C-b4 had good drying properties, solvent resistance and weather resistance, but poor appearance.
[0116] From the above, it was confirmed that the isocyanate composition of the present embodiment can provide a coating composition having good viscosity stability, and can also provide a coating film having good drying properties and solvent resistance. [Industrial Applicability]
[0117] The isocyanate composition of the present embodiment is preferably used as a curing agent for a coating composition. The coating composition can be used as a coating material for roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, and the like. The coating composition can also be used as a primer or top coat for metals such as steel plates and surface-treated steel plates, and for materials such as plastics, wood, films, and inorganic materials. The coating composition is also useful as a coating material for imparting heat resistance, cosmetic properties (surface smoothness, sharpness), etc. to precoated metals including rust-resistant steel plates, painted parts of automobiles, etc. The coating composition is also useful as a urethane raw material for adhesives, pressure sensitive adhesives, elastomers, foams, surface treatment agents, and the like.
Claims
1. The present invention includes a triisocyanate represented by the following general formula (I) and a compound represented by the following general formula (II), The isocyanate composition, wherein the content of the compound represented by the general formula (II) relative to the mass of the triisocyanate represented by the general formula (I) is 0.50 mass% or more and 5.00 mass% or less. 【Chemistry 1】 [In the general formula (I), 1 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain one or more structures selected from the group consisting of an ester structure and an ether structure. 1 may be the same or different. 1 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 【Chemistry 2】 [In general formula (II), R 2 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms. 3 is an isocyanate group.
2. 2. The isocyanate composition according to claim 1, wherein the triisocyanate represented by the general formula (I) is lysine triisocyanate.
3. The isocyanate composition according to claim 1 or 2, wherein the compound represented by the general formula (II) is p-toluenesulfonyl isocyanate.
4. A coating composition comprising the isocyanate composition according to any one of claims 1 to 3 and a polyol.
5. A coating film obtained by curing the coating composition according to claim 4.
6. A coated article comprising the coating film according to claim 5.
Citation Information
Patent Citations
Lysine ester triisocyanate
JP1978135931A
Quick-drying covering composition
JP1982198761A
Production of crosslinked resin
JP1983098326A
Thermosetting resin composition
JP1984027915A
Rapidly-drying coating composition
JP1985044561A