Patch base material and patch
A thin patch base material with a specific air permeability-to-thickness ratio addresses the issues of adherence and ingredient leakage, ensuring the patch remains in place and retains its components effectively.
Patent Information
- Application Number
- JP2020101303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-14
- Filing Date
- 2020-06-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-06-11
AI Technical Summary
Existing patch base materials with fiber sheets face issues of functional ingredients oozing out and being easily peeled off due to breathability and thickness, leading to poor adherence during use.
A patch base material with a thickness of 0.48 mm or less and an air permeability-to-thickness ratio of greater than 0 and less than 431, ensuring the patch remains adhered and prevents functional ingredients from seeping out.
The solution results in a patch that is difficult to peel off and effectively retains functional ingredients, maintaining adherence and preventing leakage during use.
Smart Images

Figure 0007591875000004 
Figure 0007591875000001 
Figure 0007591875000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a patch that is difficult to peel off during use and from which the functional ingredients it holds are difficult to ooze out, and to a patch base material capable of preparing such a patch. [Background technology]
[0002] Patches (e.g., poultices, plasters, tape preparations, surgical tapes, taping materials and bandages, facial masks, warming sheets and cooling sheets) are used in which a functional component such as an adhesive and / or a drug is applied to or impregnated into a patch base material for the purpose of, for example, exerting an anti-inflammatory and analgesic effect, exerting a cosmetic effect by cosmetics, or giving a warm or cool feeling. As a base material for a patch used for such a purpose, for example, as disclosed in JP-A-2015-190065 (Patent Document 1), a patch base material provided with a fiber sheet such as a fiber web, a nonwoven fabric, a woven fabric or a knitted fabric has been studied. Patches in which a drug-containing adhesive is applied to a support for the purpose of being applied to the human body and achieving various efficacies such as anti-inflammatory and analgesic effects are widely known as poultices, plasters, therapeutic adhesive tapes, etc. In the present invention, these are collectively referred to as "patches", and various drugs corresponding to the desired efficacy are known as such patches, and adhesives containing these drugs are applied to a support such as a nonwoven fabric, a resin film, or a composite product thereof. Patches in which an adhesive containing a drug is applied to a support for the purpose of being applied to the human body to achieve various efficacies such as anti-inflammatory and analgesic effects are widely known as poultices, plasters, therapeutic adhesive tapes, etc. In the present invention, these are collectively referred to as "patches", and various drugs corresponding to the desired efficacy are known as such patches, and adhesives containing these drugs are applied to a support such as a nonwoven fabric, a resin film, or a composite product thereof. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-190065 A (claims, 0045, etc.) Summary of the Invention [Problem to be solved by the invention]
[0004] Although such patch base materials have excellent conformability and flexibility because they are equipped with a fiber sheet, the fiber sheet is breathable, and when a functional ingredient is applied to a patch base material equipped with a fiber sheet by coating or impregnation, the applied functional ingredient sometimes passes through the fiber sheet and seeps out to the side opposite to the side to which it is applied.
[0005] One method for preventing seepage is to simply increase the thickness of the patch base material to make seepage less likely, as disclosed in Patent Document 1, but this creates a new problem in that the patch is too thick and tends to come off when it comes into contact with the human body or clothing during use.
[0006] Therefore, there has been a demand for a patch that is difficult to peel off during use and that is difficult for the functional ingredients it holds to bleed out, as well as a patch base material that can achieve this. [Means for solving the problem]
[0007] The first invention is "(Claim 1) A patch substrate having a thickness of 0.48 mm or less and equipped with a fiber sheet, the patch substrate satisfying the following formula:
[0008] Note 0<(breathability of patch base material / thickness of patch base material)<431".
[0009] The second invention is "(Claim 2) A patch comprising the patch base material according to claim 1." Effect of the Invention
[0010] The applicant of the present application has discovered that by having a thickness of a patch base material provided with a fiber sheet of 0.48 mm or less, it is possible to realize a patch that is less likely to come off during use.
[0011] The inventors then discovered that, in this patch base material, when the air permeability of the patch base material divided by the thickness of the patch base material is greater than 0 and less than 431, it is possible to realize a patch in which the retained functional ingredients are less likely to leak out, even in a patch base material with a thickness of 0.48 mm or less.
[0012] That is, the applicant of the present application discovered that there is a proportional relationship between the breathability of the patch substrate (the difficulty of gas passing through the patch substrate from one main surface to the other main surface) and the difficulty of the functional component seeping out (the difficulty of the functional component passing through the patch substrate from one main surface to the other main surface) and that the breathability of the patch substrate can be correctly evaluated by the breathability per unit thickness of the patch substrate (a value calculated by dividing the breathability of the patch substrate by the thickness of the patch substrate). That is, there is a proportional relationship between the value obtained by dividing the breathability of the patch substrate by the thickness of the patch substrate and the difficulty of the functional component seeping out.
[0013] Specifically, they discovered that a patch base having an air permeability greater than 0 and less than 431 obtained by dividing the air permeability of the patch base by the thickness of the patch base can produce a patch that is less susceptible to leakage of applied functional ingredients.
[0014] As described above, the present invention can provide a patch base material that can realize a patch that is not easily peeled off during use and from which the retained functional ingredients are not easily exuded.
[0015] Furthermore, a patch having a patch base material satisfying the configuration according to the present invention is a patch that is not easily peeled off during use and is also not susceptible to leakage of the retained functional ingredient. [Brief description of the drawings]
[0016] [Figure 1]FIG. 1 shows the arrangement of resin components in the cross section of a splittable fiber used in Example 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The patch substrate of the present invention (hereinafter, sometimes simply referred to as "substrate") has a thickness of 0.48 mm or less so that the patch is not easily peeled off during use. In other words, the thinner the substrate, the less likely it is to be caught by the periphery of the substrate constituting the patch, and the less likely the patch is to peel off during use. The thinner the substrate, the less likely it is to be caught and peeled off during use, so the thickness of the substrate is preferably 0.46 mm or less, more preferably 0.44 mm or less, and even more preferably 0.42 mm or less. The lower limit of the thickness of the substrate is not particularly limited, but is preferably 0.01 mm or more.
[0018] In the present invention, the "thickness" is defined as the area of 5 cm2 of the main surface of the substrate. 2 The thickness of the load area is measured at five randomly selected locations with a load of 0.98 N (=100 gf) per unit, and the arithmetic average of the thicknesses is calculated. Such thickness measurements can be performed, for example, with a high-precision digital length measuring instrument (Litematic (registered trademark), manufactured by Mitutoyo Corporation).
[0019] In addition, it was found that the breathability of the substrate of the present invention is proportional to the breathability of the functional component, and that the breathability of the substrate can be properly evaluated by the breathability per unit thickness of the substrate (breathability of substrate / thickness of substrate) (hereinafter, sometimes referred to as "breathability per unit thickness"). In other words, it was found that the breathability per unit thickness and the breathability of the functional component are proportional to each other. More specifically, it was found that a patch from which the functional component is less likely to leak can be realized by having a unit thickness breathability greater than 0 and less than 431. Usually, as described above, when the thickness of the substrate is thin, the structure of the substrate (particularly the fiber sheet) becomes coarse, and the breathability number becomes large, resulting in a very large unit thickness breathability. However, in the present invention, despite the thin thickness of the substrate, the structure of the substrate is dense, and the breathability number is small, so that the unit thickness breathability can be suppressed to less than 431, resulting in a substrate that can form a patch from which the functional component is less likely to leak. The smaller the unit thickness air permeability, the lower the air permeability and the less likely the functional ingredient will seep out, so the unit thickness air permeability [= (air permeability of substrate / thickness of substrate)] is preferably 420 or less, more preferably 410 or less, even more preferably 400 or less, and even more preferably 390 or less. On the other hand, as described above, a small unit thickness air permeability means that the substrate has a dense structure, but if the substrate structure is too dense, the functional ingredient-containing material such as the paste or adhesive cannot penetrate into the substrate, and the anchor effect tends to be unsatisfactory, and peeling may occur between the functional ingredient-containing material of the patch and the substrate during use of the patch, so the unit thickness air permeability is preferably 40 or more, more preferably 80 or more, and even more preferably 100 or more.
[0020] In this way, the air permeability per unit thickness of the substrate of the present invention can be calculated by dividing the air permeability of the substrate by the thickness of the substrate. 3 / cm 2 s) is measured in accordance with JIS L 1096:2010, 8.26.1 A method (Fragile type method). In other words, the measurement area is 38 cm 2Under these conditions, the air flow rate is adjusted so that the pressure is 125 Pa, and the unit time and the air permeability per unit time are measured. Such measurements of air permeability can be performed, for example, using a Frazier-type air permeability tester (product number: FX3300) manufactured by TEXTESTAG. The unit of thickness of the substrate is "mm".
[0021] The air permeability of the substrate of the present invention is not particularly limited as long as it satisfies the unit thickness air permeability. 3 / cm 2 s, preferably less than 200 cm 3 / cm 2 s or less is more preferable, and 190 cm 3 / cm 2 s or less, and more preferably 185 cm 3 / cm 2 s or less, and more preferably 170 cm 3 / cm 2 s or less, and more preferably 160 cm 3 / cm 2 s or less, and more preferably 150 cm 3 / cm 2 On the other hand, low air permeability of the substrate means that the substrate (particularly the fiber sheet) has a dense structure. If the substrate structure is too dense, the functional ingredient-containing materials such as the paste and adhesive cannot penetrate into the substrate, and the anchor effect tends to be lost. There is a possibility that peeling may occur between the functional ingredient-containing materials of the patch and the substrate during use. Therefore, the air permeability of the substrate should be 30 cm or less. 3 / cm 2 ·s or more is preferable, and 40cm 3 / cm 2 s or more is preferable, and 50 cm 3 / cm 2 s or more is more preferable, and 60 cm 3 / cm 2 It is more preferable that the value is equal to or larger than ·s.
[0022] In addition, as described above, there is a proportional relationship between the thickness of the substrate and the difficulty of peeling, and there is a proportional relationship between the air permeability and the difficulty of the functional ingredient leaking out. In addition, the thinner the substrate, the larger the air permeability value becomes, so there is an inverse proportional relationship between the thickness of the substrate and the air permeability. Therefore, when the substrate is made thin so as to be difficult to peel off and the air permeability is made small so as to be difficult to leak out, there is an inverse proportional relationship between the thickness and the air permeability, so it was found that the value obtained by multiplying the thickness and the air permeability (sometimes called the "thickness air permeability constant") falls within a certain numerical range to a certain extent. More specifically, it was found that when the thickness air permeability constant is less than 109, a patch that is difficult to peel off and difficult to leak out can be prepared. A thinner film is less likely to peel off, and a smaller air permeability is less likely to cause the functional component to seep out, and as a result, the smaller the thickness air permeability constant, the better the above-mentioned effect, so the thickness air permeability constant is preferably 100 or less, more preferably 90 or less, even more preferably 80 or less, even more preferably 70 or less, and even more preferably 60 or less. The lower limit of the thickness air permeability constant is not particularly limited, and it is sufficient if it is greater than 0, and is preferably 1 or more.
[0023] The substrate of the present invention preferably has a small surface dynamic friction coefficient so that the patch is difficult to peel off when it comes into contact with the human body or clothing during use.In other words, if the surface dynamic friction coefficient is large, the force of contact with the human body or clothing is easily applied to the patch, making it easy to peel off, so the surface dynamic friction coefficient is preferably small.Specifically, the surface dynamic friction coefficient is preferably 0.5 or less.
[0024] This "surface dynamic friction coefficient" is a value obtained based on JIS K 7125:1999. Specifically, it is measured using a static and dynamic friction measuring device (manufactured by Trinity Lab Co., Ltd., product number: TL201Tt) and a contact terminal (area: 1 cm 2 ) is set with cotton No. 3-1 as specified in JIS L 0803, and a load of 100 g is applied while tracing the surface of the substrate at a speed of 10 mm / sec. The dynamic friction coefficient calculated based on the obtained data is regarded as the "surface dynamic friction coefficient."
[0025] The substrate of the present invention has a tensile strength of preferably 5N / (50mm width) or more in both the vertical and horizontal directions, more preferably 10N / (50mm width) or more, even more preferably 15N / (50mm width) or more, and even more preferably 20N / (50mm width) or more, so that the substrate does not break when the patch is applied incorrectly or when it is peeled off after use. The upper limit of the tensile strength is not particularly limited, but since the substrate tends to become hard when the tensile strength is high, it is preferably 300N / (50mm width) or less, and more preferably 200N / (50mm width) or less. In addition, in order that the base material has approximately the same tensile strength in both the vertical and horizontal directions and that the patch can be peeled off without directional breakage, the ratio of the vertical tensile strength (Tm) to the horizontal tensile strength (Tc) (=Tm / Tc) is preferably 0.4 to 2.5, more preferably 0.6 to 2.3, and even more preferably 0.8 to 2.1.
[0026] The "tensile strength" is measured by taking a rectangular sample piece 50 mm wide and 250 mm long from the substrate, pulling the rectangular sample piece in the long side direction using a constant speed extension tensile tester (Tensilon, manufactured by Orientec Co., Ltd.), and measuring the maximum load until the test piece breaks. This maximum load measurement is performed for three sample pieces, and the arithmetic average of these maximum loads is taken as the "tensile strength". The measurement is performed under conditions of a gripping distance of 200 mm and a pulling speed of 500 mm / min. In the present invention, the "vertical direction" refers to the production direction (flow direction) during the production of the substrate, and the "horizontal direction" refers to the direction perpendicular to the vertical direction, that is, the width direction.
[0027] The more stretchable the substrate of the present invention is, the better its adhesion to the skin or other object, so the elongation in both the vertical and horizontal directions is preferably 5% or more, more preferably 15% or more, even more preferably 25% or more, and even more preferably 25% or more. Although there is no particular upper limit to the elongation, a high elongation tends to result in poor shape stability, so it is preferably 400% or less, more preferably 350% or less, even more preferably 300% or less, even more preferably 275% or less, and even more preferably 250% or less. Furthermore, in order that the base material has approximately the same elongation in both the vertical and horizontal directions and that the patch can adhere closely to the target object without any directional tendency, the ratio of the elongation in the vertical direction (Em) to the elongation in the horizontal direction (Ec) (=Em / Ec) is preferably 0.5 to 2.0, more preferably 0.6 to 1.7, and even more preferably 0.8 to 1.3.
[0028] This elongation (Sr, unit: %) refers to the percentage of the elongation of the sample piece at the maximum load (Smax, unit: mm) [= (length at the maximum load, unit: mm) - (grip interval = 200 mm)] relative to the grip interval (200 mm) when the above-mentioned tensile strength measurement was performed. In other words, it is a value obtained from the following formula. This measurement was performed three times, and the arithmetic average of the percentages is defined as the elongation in the present invention. Sr = (Smax / 200) x 100
[0029] In order to make the substrate of the present invention stretch easily and have excellent adhesion to objects such as the skin, the tensile strength at 20% elongation in both the longitudinal and transverse directions is preferably 10 N / (5 cm width) or less, more preferably 9 N / (5 cm width) or less, even more preferably 8 N / (5 cm width) or less, and even more preferably 7 N / (5 cm width) or less. If the tensile strength at 20% elongation is too low, the shape stability tends to be poor, so the tensile strength is preferably 0.1 N / (5 cm width) or more, more preferably 0.2 N / (5 cm width) or more, and even more preferably 0.5 N / (5 cm width) or more. Furthermore, in order that the base material is easily stretched to the same extent in both the vertical and horizontal directions and that the patch can adhere to the target object without directional tendency, the ratio (=Mm / Mc) of the tensile strength (Mm) at 20% elongation in the vertical direction to the tensile strength (Mc) at 20% elongation in the horizontal direction is preferably 0.5 to 2.0, more preferably 0.6 to 1.7, and even more preferably 0.8 to 1.3.
[0030] The tensile strength at 20% elongation is measured by taking a sample piece 50 mm wide and 250 mm long from the substrate, and using a constant-speed extension tensile tester (Tensilon, manufactured by Orientec Co., Ltd.), fixing the sample piece with a gripping distance of 200 mm, and measuring the load at the point of elongation of 40 mm (=20%) (grip distance: 240 mm). This load measurement is performed for three sample pieces, and the arithmetic average of these loads is taken as the "tensile strength at 20% elongation." The measurement is performed at a pulling speed of 500 mm / min.
[0031] The substrate of the present invention is easy to stretch, and in order to have excellent adhesion to objects that require large stretching such as elbows and knees, and to provide an excellent feeling of application, the tensile strength at 50% elongation in either the vertical or horizontal direction is preferably 30 N / (5 cm width) or less, more preferably 15 N / (5 cm width) or less, even more preferably 10 N / (5 cm width) or less, and even more preferably 5 N / (5 cm width) or less. If the tensile strength at 50% elongation is too low, the shape stability tends to be poor, so it is preferably 0.1 N / (5 cm width) or more, and more preferably 0.5 N / (5 cm width) or more. In addition, in order that the base material can stretch to the same extent in both the vertical and horizontal directions and that the patch can adhere to the target object without directional tendency, the ratio (=Mm / Mc) of the tensile strength (Mm) at 50% elongation in the vertical direction to the tensile strength (Mc) at 50% elongation in the horizontal direction is preferably 0.5 to 2.0, and more preferably 0.6 to 1.7.
[0032] The tensile strength at 50% elongation is measured by taking a sample piece 50 mm wide and 250 mm long from the substrate, and using a constant-speed extension tensile tester (Tensilon, manufactured by Orientec Co., Ltd.), fixing the sample piece with a gripping distance of 200 mm, and measuring the load at the point of elongation of 100 mm (=50%) (grip distance: 300 mm). This load measurement is performed for three sample pieces, and the arithmetic average of these loads is taken as the "tensile strength at 50% elongation." The measurement is performed at a pulling speed of 500 mm / min.
[0033] The base material of the present invention expands and contracts in accordance with the movement of the subject such as the skin, so that the adhesion between the subject and the patch is maintained and the patch is not easily peeled off from the subject when used, and the recovery rate at 20% elongation in both the vertical and horizontal directions is preferably 25% or more, more preferably 30% or more, even more preferably 40% or more, and even more preferably 50% or more. In addition, the ratio of the recovery rate at 20% elongation in the vertical direction (Rm) to the recovery rate at 20% elongation in the horizontal direction (Rc) (=Rm / Rc) is preferably 0.5 to 2.0, more preferably 0.6 to 1.7, and even more preferably 0.7 to 1.4, so that the base material is easily expandable in both the vertical and horizontal directions, the adhesion between the subject and the patch is maintained, and the patch is not easily peeled off from the subject when used.
[0034] This recovery rate at 20% elongation is a value obtained by the following procedure. First, a sample piece with a width of 50 mm and a length of 250 mm is taken from the substrate, and the test piece is fixed with a gripping distance of 200 mm using a constant-speed extension tensile tester (Tensilon, manufactured by Orientec Co., Ltd.). The gripping distance of 200 mm is set as the starting point, and a position 40 mm from the starting point (= 20% elongation position, elongation L 20 The specimen is pulled at a speed of 500 mm / min to a tension of 0.05 N (Lf = 40), and then returned to the starting point at the same speed. The elongation (Lf) when the tensile stress of the substrate becomes 0.05 N during this pulling operation, and the elongation (Lb) when the tensile stress of the substrate becomes 0.05 N during the return operation are measured. This measurement is carried out for three test pieces, and the elongations (Lf, Lb) are arithmetically averaged to obtain the average elongation (Lf) during the pulling operation. av ) and the average elongation during return operation (Lb av The value calculated from the following formula is the recovery rate at 20% elongation (R, unit: %). R = {(L 20 -Lf av )-(Lb av -Lf av )} / (L 20 -Lf av ) x 100
[0035] The base material of the present invention can expand and contract in accordance with the movement of an object that requires large stretching, such as an elbow or knee, thereby maintaining adhesion between the object and the patch and making it difficult for the patch to peel off from the object when in use. In order to achieve this, the recovery rate at 50% elongation in either the vertical or horizontal direction is preferably 25% or more, more preferably 30% or more, even more preferably 35% or more, and even more preferably 40% or more.
[0036] This recovery rate at 50% elongation is a value obtained by the following procedure. First, a sample piece with a width of 50 mm and a length of 250 mm is taken from the substrate, and the test piece is fixed with a gripping distance of 200 mm using a constant-speed extension tensile tester (Tensilon, manufactured by Orientec Co., Ltd.). The gripping distance of 200 mm is set as the starting point, and a position 100 mm from the starting point (= 50% elongation position, elongation L 50 The specimen is pulled at a speed of 500 mm / min to a tension point (Lf = 100), and then returned to the starting point at the same speed. The elongation (Lf) when the tensile stress of the substrate becomes 0.05 N during this pulling operation, and the elongation (Lb) when the tensile stress of the substrate becomes 0.05 N during the returning operation are measured. This measurement is carried out for three test pieces, and the elongations (Lf, Lb) are arithmetically averaged to determine the average elongation (Lf) during the pulling operation. av ) and the average elongation during return operation (Lb av The value calculated from the following formula is the "50% elongation recovery rate (R, unit: %)." R = {(L 50 -Lf av )-(Lb av -Lf av )} / (L 50 -Lf av ) x 100
[0037] The basis weight of the substrate of the present invention is not particularly limited as long as it satisfies the above-mentioned thickness and unit thickness air permeability. 2 It is preferable that the thickness is less than 70 g / m 2 More preferably, it is 60 g / m or less. 2The lower limit of the basis weight of the substrate is not particularly limited, but it is preferably 1 g / m or less so that the above-mentioned unit thickness air permeability can be easily satisfied. 2 It is preferable that the thickness is 5 g / m or more. 2 More preferably, it is 10 g / m or more. 2 More preferably, the above is true.
[0038] In the present invention, the basis weight is calculated by taking three test pieces of 10 cm square from the substrate, measuring the mass of each test piece, and then calculating the arithmetic average of the masses of the three test pieces. 2 The value converted into the mass per unit area is called the basis weight.
[0039] The substrate of the present invention is provided with a fiber sheet, so that it can hold functional ingredients and form a patch. The fiber sheet constituting the substrate of the present invention is not particularly limited, but can be, for example, a nonwoven fabric, a woven fabric, a knitted fabric, or a composite of these. In particular, the nonwoven fabric can have a dense structure due to the uniform dispersion of fibers, and is easy to satisfy the unit thickness air permeability, so it is preferable to include a nonwoven fabric as the fiber sheet. When the fiber sheet includes a suitable nonwoven fabric, it may be a dry nonwoven fabric or a wet nonwoven fabric, but it is preferable to use a wet nonwoven fabric because it can have a dense structure even if it is thin in thickness, with fibers more uniformly dispersed. The substrate of the present invention can be composed of only a fiber sheet, or may be provided with a porous film, net, etc. in addition to the fiber sheet, but if it is composed of only a fiber sheet, the thickness of the substrate is thinner, it is less likely to get caught at the periphery of the substrate, and the patch is less likely to peel off during use, so it is preferable.
[0040] The substrate of the present invention may have a partially bonded portion. If the bonded portion is information on the source, medicinal components, design, etc., the information can be recognized. This "bonded portion" is usually formed on a fiber sheet, but it is preferable that the fibers are not fused. By not being fused, the flexibility of the substrate is not impaired, and a patch with excellent adhesion to the target object can be produced.
[0041] Furthermore, information such as the source, medicinal components, and design may be printed on the base material of the present invention.
[0042] Additionally, the substrate of the present invention may be colored with a pigment or dye.
[0043] The fibers constituting the fiber sheet of the present invention are not particularly limited, but since the smaller the fiber diameter, the easier it is for the substrate provided with the fiber sheet to satisfy the thickness and unit thickness air permeability, it is preferable for the fiber sheet to contain fine fibers having a fiber diameter of 6 μm or less, more preferably fine fibers having a fiber diameter of 5 μm or less, even more preferably fine fibers having a fiber diameter of 4.5 μm or less, even more preferably fine fibers having a fiber diameter of 4 μm or less, and even more preferably fine fibers having a fiber diameter of 3 μm or less. The lower limit of the fiber diameter of the fine fibers is not particularly limited, but it is preferably 0.1 μm or more.
[0044] Such suitable fine fibers may be commercially available fibers (e.g., Tepyrus (registered trademark)), may be fibers formed by melt-blowing, or may be fibers generated from splittable fibers formed by mixed spinning or composite spinning and capable of being split by physical and / or chemical treatment. Among these, commercially available fibers and fibers generated from splittable fibers are suitable because they have been mechanically stretched, and therefore have excellent fiber strength, and are unlikely to fall off from the substrate due to friction during use of the patch. Examples of physical treatments for splitting splittable fibers include, for example, a fluid flow such as a water flow, a needle, a calendar, and the like, and examples of chemical treatments include, for example, dissolving and removing resin components with a solvent, and swelling resin components with a solvent. Among these, fine fibers split by physical treatments are preferred because they can be a fiber sheet with excellent density and low air permeability.
[0045] The resin component constituting such fine fibers may be any one that is not damaged by the functional component and does not absorb or adsorb the functional component, and is not particularly limited since it differs depending on the functional component, but may be, for example, regenerated fibers such as rayon and cupra, semi-synthetic fibers such as acetate and promix, synthetic fibers such as nylon, vinylon, vinylidene, polyvinyl chloride, polyester, acrylic, polyethylene, polypropylene, polyurethane, vegetable fibers such as cotton and hemp, and animal fibers such as wool and silk. For example, when preparing a patch containing an anti-inflammatory and analgesic component such as methyl salicylate, ketoprofen, or loxonin as a functional component, the fine fibers constituting the fiber sheet are preferably composed of polyester resin or polypropylene resin that is less likely to cause drug adsorption.
[0046] In the present invention, the "fiber diameter" refers to the diameter of a fiber when the cross-sectional shape is circular, and when the cross-sectional shape is other than circular, the fiber diameter is regarded as the diameter of a circle having the same area as the cross-sectional area.
[0047] In addition, the fiber constituting the fiber sheet of the present invention preferably contains highly crimped fibers in which the crimp of the latent crimped fiber is expressed. This is because such highly crimped fibers, when they express crimp, cause entanglement with adjacent fibers, so that the fibers are in close contact with each other, resulting in a fiber sheet having a dense structure, and as a result, a substrate having a dense structure. In addition, by containing such highly crimped fibers, the effect of excellent flexibility and elasticity and less fuzzing due to friction is also achieved. Even in such a high crimp, if the fiber diameter of the latent crimped fiber itself is large and thick, it tends to be difficult to simultaneously satisfy the above-mentioned thickness and unit thickness air permeability, so the fiber diameter of the latent crimped fiber is preferably 13 μm or less, more preferably 12 μm or less, and even more preferably 11 μm or less. The lower limit of the fiber diameter of the latent crimped fiber is not particularly limited, but it is preferably 0.1 μm or more.
[0048] Examples of such latent crimp fibers include (1) composite fibers in which a plurality of resins with different thermal shrinkage rates are combined in an eccentric core-sheath or side-by-side configuration, and which exhibit crimping when heated; (2) fibers in which a specific heat history is applied to a part of the fiber, and which exhibit crimping when heated; and (3) eccentric hollow fibers that are made of one type of resin component but have a hollow portion extending in the length direction of the fiber in an eccentric state, and which exhibit crimping when heated. Examples of the resin combinations of the composite fibers in (1) include polyester-copolyester, polyamide-copolyamide, polyester-polyamide, polyester-polypropylene, polypropylene-copolypropylene, and polypropylene-polyethylene. When the substrate is required to have chemical resistance, flexibility, and / or stretchability, latent crimp fibers made of a combination of polyester-copolyester or polypropylene-low melting point polypropylene are preferred. As the latent crimped fiber of (2) in which a part of the fiber has been subjected to a specific heat history, for example, a fiber made of a thermoplastic resin such as polyester or polyamide, which is passed through a hot blade or the like, can be used. Furthermore, as the eccentric hollow fiber of (3) above, for example, it can be made of a thermoplastic resin such as polyester, polypropylene, or polyamide. When preparing a patch containing an anti-inflammatory and analgesic ingredient such as methyl salicylate, ketoprofen, or loxonin as a functional ingredient, it is preferable that the latent crimped fiber constituting the fiber sheet is made of a polyester resin, a copolymer polyester resin, a polypropylene resin, and / or a copolymer polypropylene resin, which are unlikely to cause drug adsorption.
[0049] Furthermore, the fibers constituting the fiber sheet of the present invention may contain adhesive fibers. By bonding the adhesive fibers, it is expected that the fibers are less likely to fall off the substrate due to friction during use of the patch. In addition, by bonding the adhesive fibers, even if physical treatment such as water flow is performed, the fibers are not rearranged, and a dense structure in which the fibers are uniformly distributed can be obtained. Even with such adhesive fibers, if the fiber diameter of the adhesive fiber itself is large and thick, it tends to be difficult to simultaneously satisfy the above-mentioned thickness and unit thickness air permeability, so the fiber diameter of the adhesive fiber is preferably 13 μm or less, more preferably 12 μm or less, and even more preferably 11 μm or less. The lower limit of the fiber diameter of the adhesive fiber is not particularly limited, but it is preferably 0.1 μm or more.
[0050] Such adhesive fibers can be full melt type fibers, or composite fibers such as core-sheath type, sea-island type, and side-by-side type in which the low melting point component is exposed on the surface of the fiber. When the adhesive fibers are composite fibers, the fiber form is maintained, and the density of the fiber sheet and therefore the density of the substrate are excellent. The components other than the low melting point component (high melting point components) of the adhesive fibers made of composite fibers preferably have a melting point 5°C or higher than the low melting point component so that the fiber form can be maintained, more preferably a melting point 10°C or higher, and even more preferably a melting point 15°C or higher.
[0051] The adhesive fiber can be made of a thermoplastic resin, such as polyester, copolymerized polyester, polyamide, copolymerized polyamide, polypropylene, copolymerized polypropylene, polyethylene, copolymerized polyethylene, etc. When the adhesive fiber is made of a composite fiber, the combination of resins can be, for example, polyester-copolymerized polyester, polyester-polyamide, polyester-copolymerized polyamide, polyester-polypropylene, polyester-copolymerized polypropylene, polyester-polyethylene, polyester-copolymerized polyethylene, polyamide-copolymerized polyester, polyamide-copolymerized polyamide, polyamide-polypropylene, polyamide-copolymerized polypropylene, polyamide-polyethylene, polyamide-copolymerized polyethylene, polypropylene-copolymerized polypropylene, polypropylene-polyethylene, polypropylene-copolymerized polyethylene, polyethylene-copolymerized polyethylene, etc. For example, when preparing a patch containing an anti-inflammatory and analgesic component such as methyl salicylate, ketoprofen, or loxonin as a functional component, the adhesive fiber constituting the fiber sheet is preferably made of a polyester resin, a copolymerized polyester resin, a polypropylene resin, and / or a copolymerized polypropylene resin, which are less likely to cause drug adsorption.
[0052] The fiber lengths of the above-mentioned fine fibers, highly crimped fibers, and adhesive fibers vary depending on the structure of the fiber sheet and are not particularly limited; however, for example, when the fiber sheet is made of a dry nonwoven fabric, excessively long fiber lengths deteriorate the carding properties, increase unopened fibers and neps, and deteriorate the texture, resulting in greater variation in fiber dispersion and partially increased breathability that tends to facilitate seepage of functional ingredients. Therefore, the fiber lengths are preferably 110 mm or less, more preferably 100 mm or less, even more preferably 90 mm or less, and even more preferably 80 mm or less. On the other hand, if the fiber length is too short, the strength of the fiber web will be weak, and the texture will deteriorate during the nonwoven fabric formation process, resulting in greater variation in fiber distribution and increased localized breathability, which will tend to facilitate seepage of functional ingredients. In addition, the strength of the dry nonwoven fabric itself will also tend to be weakened, so the fiber length is preferably 10 mm or more, more preferably 20 mm or more, and even more preferably 30 mm or more.
[0053] In addition, when the fiber sheet is a wetlaid nonwoven fabric, the fibers are uniformly dispersed and have a dense structure, and thus the substrate has excellent density and the functional components are unlikely to seep out, so that the fiber length of the fibers constituting the wetlaid nonwoven fabric is preferably 40 mm or less, more preferably 30 mm or less, even more preferably 20 mm or less, even more preferably 15 mm or less, and even more preferably 10 mm or less. On the other hand, the fiber length of the fibers constituting the wetlaid nonwoven fabric is preferably 0.1 mm or more, so that the substrate has strength, excellent density, and the functional components are unlikely to seep out.
[0054] The cross-sectional shape of the above-mentioned fine fibers, highly crimped fibers, and adhesive fibers is not particularly limited, and examples thereof include a perfect circle, an oval, an ellipse, a polygon (e.g., a triangular shape, a rectangular shape, a trapezoidal shape, etc., a pentagonal shape, a hexagonal shape, etc.), and an alphabet shape (e.g., an E shape, an F shape, an H shape, an I shape, a K shape, an L shape, an M shape, an N shape, a T shape, an X shape, a Y shape, etc.). In particular, when the cross-sectional shape of a triangular shape, a rectangular shape, an I shape, etc. has a large flattening ratio [= (shortest length that can be taken in the cross section) / (longest length that can be taken in the cross section)×100], the fiber sheet can have a dense structure, and thus the substrate can have a dense structure, which is preferable.
[0055] Furthermore, the fine fibers, highly crimped fibers, and adhesive fibers described above can be white, but they may be colored with a pigment and / or dye other than white. For example, when used as a base material for a skin patch, it is preferable to color them in a flesh color, since they are not noticeable when the patch is applied to the skin.
[0056] The fiber sheet of the present invention preferably contains, as constituent fibers, fine fibers, highly crimped fibers, and adhesive fibers as described above, but may contain fibers that do not fall within the categories of these fibers, such as synthetic fibers such as polyester fibers (polyethylene terephthalate fibers, polybutylene terephthalate fibers, polytrimethylene terephthalate fibers, etc.), polyolefin fibers (polyethylene fibers, polypropylene fibers, etc.), polyamide fibers (nylon 6 fibers, nylon 66 fibers, etc.), polyvinyl alcohol fibers, and acrylic fibers, or cellulosic fibers such as cotton and rayon.
[0057] The fiber sheet of the present invention can be composed of the fibers described above, and since the smaller the average fiber diameter of the fibers constituting the fiber sheet, the denser the structure of the fiber sheet can be, and the easier it is to simultaneously satisfy the thickness and unit thickness air permeability described above, the average fiber diameter of the fibers constituting the fiber sheet is preferably 14 μm or less, more preferably 13 μm or less, and even more preferably 12 μm or less. The lower limit of the average fiber diameter of the fibers constituting the fiber sheet is not particularly limited, but is preferably 0.1 μm or more.
[0058] The "average fiber diameter" in the present invention is a value obtained by the following method. (1) The total fiber length of each type of fiber (Lt1, Lt2, . . ., Lt n ) are calculated respectively. (2) The total fiber length of each type of fiber in (1) (Lt1, Lt2, . . ., Lt n ), the total fiber length of all the fibers constituting the fiber sheet (= Ltt = Lt1 + Lt2 + + Lt n ) is calculated. (3) The ratio of the total fiber length of each type of fiber to the total fiber length of all fibers constituting the fiber sheet (=Ltt) (Rl1=Lt1 / Ltt, Rl2=Lt2 / Ltt, . . ., Rl n =Lt n / Ltt) are calculated respectively. (4) The fiber diameter of each type of fiber (D1, D2, . . ., D n ) and (3) the ratio of the total fiber length of each type of fiber (Rl1, Rl2, . . ., Rl n ) The value obtained by the following formula is the average fiber diameter (Da). Da = D1 × Rl1 + D2 × Rl2 + + D n ×Rl n
[0059] As described above, the substrate of the present invention can provide a patch that is not easily peeled off during use and does not easily ooze out the functional components it holds, and therefore can be suitably used as a base fabric for patches to be attached to the human body. More specifically, it can be used as a substrate for patches that hold functional components for the purpose of exerting anti-inflammatory and analgesic effects, exerting cosmetic effects as cosmetics, or giving a warm or cool sensation, such as poultices, plasters, tape preparations, surgical tapes, taping materials and bandages, facial masks, and warming and cooling sheets.
[0060] The fiber sheet constituting the substrate of the present invention can be produced using, for example, fine fibers, latent crimp fibers and / or adhesive fibers.
[0061] For example, a suitable nonwoven fabric can be produced by forming a fiber web using fine fibers, latent crimp fibers, and / or adhesive fibers by a dry or wet method, and then bonding the fibers together and adjusting the thickness.
[0062] (Example 1) A fiber web containing latent crimped fibers is formed by a dry or wet method using relatively fine latent crimped fibers with a fiber diameter of 13 μm or less, and then entangled with a fluid flow such as a water flow or a needle. The entangled fiber web is then shrunk when the crimp of the latent crimped fibers is expressed to form highly crimped fibers. Then, the thickness is adjusted to form a nonwoven fabric having a thickness of 0.48 mm or less and a unit thickness air permeability of less than 431, and this nonwoven fabric is used as a substrate. In this specific example, a nonwoven fabric (substrate) having a dense structure, which is not easily peeled off during use, and which is not easily exuded of functional components can be manufactured by using relatively fine latent crimped fibers and adjusting the thickness.
[0063] In addition to the latent crimp fibers, splittable fibers, fine fibers and / or adhesive fibers may be included.
[0064] Furthermore, when the fiber web is formed by a wet method, it is preferable to form a wet-laid nonwoven fabric having a denser structure in which the fibers are more uniformly dispersed even if the web is thin.
[0065] Furthermore, the orientation direction of the fibers constituting the fiber web is not particularly limited, but can be, for example, a parallel web oriented in the vertical direction, a cross web in which parallel webs are oriented in the horizontal direction by a cross layer or the like, a criss-cross web in which parallel webs and cross webs are laminated, or a random web.
[0066] Furthermore, the area shrinkage rate of the entangled fiber web is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more so that the nonwoven fabric has a dense structure. This shrinkage makes it possible to obtain a soft and highly stretchable nonwoven fabric, which is a suitable embodiment for producing a nonwoven fabric (base fabric) for a patch (e.g., a medicinal patch) to be applied to the skin. In this case, if the shrinkage rate in the vertical or horizontal direction is increased, the recovery rate at 20% elongation and the recovery rate at 50% elongation in that direction can be increased, and the tensile strength at 20% elongation and the tensile strength at 50% elongation can be decreased. If the shrinkage rate is increased, the basis weight and thickness increase, so in order to obtain a base material with the desired basis weight and thickness, it is necessary to appropriately adjust, such as by decreasing the basis weight of the fiber web before shrinkage.
[0067] (Example 2) Using splittable fibers that can be split by physical treatment, a fiber web containing the splittable fibers is formed by a dry method or a wet method, and then the splittable fibers are entangled by a fluid flow such as a water flow or a needle, and at the same time, the splittable fibers are split to generate fine fibers having a fiber diameter of 6 μm or less. Then, the thickness is adjusted to form a nonwoven fabric having a thickness of 0.48 mm or less and a unit thickness air permeability of less than 431, and this nonwoven fabric is used as a substrate. In this specific example, by generating fine fibers and adjusting the thickness, a nonwoven fabric (substrate) having a dense structure, which is not easily peeled off during use, and which is not easily exuded of functional components can be manufactured.
[0068] In addition to the splittable fibers, the fabric may contain potentially crimped fibers, fine fibers and / or adhesive fibers.
[0069] In addition, the fibers may be splittable by chemical treatment rather than by physical treatment, although the fibers are preferred from the viewpoint of the denseness of the nonwoven fabric.
[0070] Furthermore, when the fiber web is formed by a wet method, it is preferable to form a wet-laid nonwoven fabric having a denser structure in which the fibers are more uniformly dispersed even if the web is thin.
[0071] Furthermore, the orientation direction of the fibers constituting the fiber web is not particularly limited, but can be, for example, a parallel web oriented in the vertical direction, a cross web in which parallel webs are oriented in the horizontal direction by a cross layer or the like, a criss-cross web in which parallel webs and cross webs are laminated, or a random web.
[0072] (Example 3) Using fine fibers with a fiber diameter of 6 μm or less, a fiber web containing the fine fibers is formed by a dry method or a wet method, and the fibers are then bonded to each other by a fluid flow such as a water flow, a needle, and / or fiber adhesion. Then, the thickness is adjusted to form a nonwoven fabric having a thickness of 0.48 mm or less and a unit thickness air permeability of less than 431, and this nonwoven fabric is used as a substrate. In this specific example, by using fine fibers and adjusting the thickness, a nonwoven fabric (substrate) having a dense structure, which is not easily peeled off during use, and which is not easily exuded of functional ingredients can be produced.
[0073] In addition to the fine fibers, the material may contain potentially crimped fibers, splittable fibers and / or adhesive fibers.
[0074] Furthermore, when the fiber web is formed by a wet method, it is preferable to form a wet-laid nonwoven fabric having a denser structure in which the fibers are more uniformly dispersed even if the web is thin.
[0075] Furthermore, the orientation direction of the fibers constituting the fiber web is not particularly limited, but can be, for example, a parallel web oriented in the vertical direction, a cross web in which parallel webs are oriented in the horizontal direction by a cross layer or the like, a criss-cross web in which parallel webs and cross webs are laminated, or a random web.
[0076] Furthermore, when the fibers are bonded together by both the fluid flow and fiber adhesion, it is preferable to perform entanglement by the fluid flow after fiber adhesion, because by previously bonding the fibers together by fiber adhesion, rearrangement of the fibers during entanglement by the fluid flow can be suppressed and uniform dispersion of the fibers can be maintained.
[0077] (Example 4) Using fine fibers having a fiber diameter of 6 μm or less, a fiber web containing the fine fibers is formed by a dry method or a wet method, and the fibers are bonded to each other by a fluid flow such as a water flow, needles and / or fiber adhesion to form a supported nonwoven fabric. Then, a fiber layer containing fine fibers, latent crimp fibers, splittable fibers and / or adhesive fibers is formed on the supported nonwoven fabric by a dry method or a wet method, and the supported nonwoven fabric and the fiber layer are bonded by a fluid flow such as a water flow, needles and / or fiber adhesion. Then, the thickness is adjusted to form a laminated nonwoven fabric having a thickness of 0.48 mm or less and a unit thickness air permeability of less than 431, and this laminated nonwoven fabric is used as a substrate. In this specific example, the supporting nonwoven fabric is formed using fine fibers, so that the supporting nonwoven fabric itself is dense, and since a fiber layer is formed on the supporting nonwoven fabric, it can be made denser, and since the thickness is adjusted, a laminated nonwoven fabric (substrate) having a dense structure, which is not easily peeled off during use, and is not easily exuded with functional components can be produced.
[0078] Incidentally, the supporting nonwoven fabric does not need to contain fine fibers, but it is preferable for the supporting nonwoven fabric to contain fine fibers, since the thickness of the supporting nonwoven fabric can be made thinner if the supporting nonwoven fabric contains fine fibers, which makes it easier to produce a patch that is less likely to peel off during use.
[0079] In addition, when a fiber web is formed by a wet method and a supporting nonwoven fabric is formed, the fibers are more uniformly dispersed even if the thickness is thin, and a supporting nonwoven fabric having a denser structure can be formed, which is preferable. Similarly, when a fiber layer is formed by a wet method, a laminated nonwoven fabric having a denser structure can be formed, which is preferable. In particular, when fibers dispersed in a slurry are woven onto a supporting nonwoven fabric, the slurry is discharged through the pores of the supporting nonwoven fabric, and the fibers in the slurry block the pores of the supporting nonwoven fabric, resulting in a denser structure, which reduces the air permeability of the laminated nonwoven fabric (substrate), and is preferable because it effectively suppresses the seepage of functional components.
[0080] Furthermore, the orientation directions of the fibers constituting the supporting nonwoven fabric and the fibers constituting the fiber layer are not particularly limited, but may be, for example, a parallel web oriented in the vertical direction, a cross web in which parallel webs are oriented in the horizontal direction by a cross layer or the like, a criss-cross web in which parallel webs and cross webs are laminated, or a random web. The orientation directions of the fibers constituting the supporting nonwoven fabric and the fibers constituting the fiber layer may be the same or different.
[0081] Furthermore, the fibers are preferably bonded to form the support nonwoven fabric by fiber adhesion which does not disturb the texture of the fibrous web.
[0082] Furthermore, the method of bonding the supporting nonwoven fabric and the fiber layer is preferably entangled with a fluid flow such as a water flow so that the supporting nonwoven fabric and the fiber layer are firmly bonded and the laminated nonwoven fabric itself is less likely to delaminate when the patch is used. When entangled with a fluid flow like this, the fibers tend to rearrange and the texture tends to be disturbed, so the supporting nonwoven fabric is preferably bonded by fiber adhesion so that the texture is less likely to be disturbed.
[0083] The specific examples described above are suitable methods for producing a nonwoven fabric that can constitute the substrate of the present invention. In order to add value to the fiber sheet containing the nonwoven fabric, post-processing such as coloring, embossing, and / or printing can also be carried out.
[0084] The coloring treatment can be a treatment of coloring the fiber sheet with a pigment or a dyeing treatment. It is also possible to manufacture a fiber sheet using fibers colored with a pigment or dyed fibers.
[0085] The embossing process is preferably performed by pressing the fibers constituting the fiber sheet without fusing them. If the fibers are fused, they tend to become hard and lose flexibility. In order not to fuse the fibers, the temperature in the embossing device is set to a temperature lower than the melting point of the resin component having the lowest melting point among the fibers constituting the fiber sheet, preferably a temperature lower than the melting point by 30°C or more, more preferably a temperature lower than the melting point by 50°C or more. On the other hand, when information is imparted to the fiber sheet by pressing, it is preferable to perform the embossing process at a temperature higher than the glass transition temperature of the resin component having the highest glass transition temperature among the fibers constituting the fiber sheet so that the information can be clearly recognized.
[0086] The printing process can be carried out by a general printing method such as gravure printing, offset printing, inkjet printing, etc., to print characters or figures on the surface of the fiber sheet. As the ink for printing, for example, inorganic pigments, organic pigments, and organic dyes can be used alone or in combination. By printing in this manner, it is possible to impart information to the fiber sheet and improve the design, as in the case of embossing.
[0087] In addition, when the substrate of the present invention includes other materials such as a porous film or net in addition to the fiber sheet, the substrate of the present invention can be manufactured by integrating the other materials with the fiber sheet. For example, the fiber sheet can be integrated with the other materials by a fluid flow such as a water flow, a needle, fiber adhesion and / or a binder. The fiber sheet may be integrated with the other materials after it is formed, or may be integrated with the other materials at the stage of forming the fiber sheet. For example, as in Example 4, the other materials can be integrated with the fiber web at the same time as the nonwoven fabric layer is formed by laminating the other materials and the fiber web and then applying a fluid flow.
[0088] Since the patch of the present invention has the above-mentioned base material, it is a patch that is not easily peeled off during use and does not easily exude the functional components that it holds. More specifically, the patch of the present invention is a patch (e.g., a cataplasm, a plaster, a tape preparation, a surgical tape, a taping material or bandage, a facial mask, a warming sheet or a cooling sheet) in which a functional component such as an adhesive and / or a drug is added to the above-mentioned base material for the purpose of exerting an anti-inflammatory and analgesic effect, exerting a cosmetic effect by a cosmetic, or giving a warm or cold feeling.
[0089] The functional ingredient of the patch is appropriately selected depending on the intended use of the patch, and is not particularly limited. For example, the functional ingredient of the patch intended for treatment may be an antipyretic analgesic and anti-inflammatory agent, a cardiac stimulant, a vitamin preparation, a cardiac drug (vasodilator), a bronchodilator, a local anesthetic, an antipruritic agent, an agent for suppurative diseases, a hormone drug, etc.; the functional ingredient of the patch intended for cosmetic effects may be a functional ingredient that has a mild effect on the human body and is defined as a quasi-drug or cosmetic, such as a beauty essence or lotion; the functional ingredient of the patch intended for a warming sensation may be a functional ingredient such as capsicum extract or benzyl nicotinate; and the functional ingredient of the patch intended for a cooling sensation may be a functional ingredient such as a cooling agent, such as a hydrous gel or menthol.
[0090] When the functional component needs to have adhesive properties, for example, a gel composition containing the functional component, such as an acrylic adhesive, a rubber adhesive, or a silicone adhesive, can be used.
[0091] The patch of the present invention can be produced by directly applying or impregnating the functional ingredient into a substrate (particularly a fiber sheet), or by applying the functional ingredient onto a carrier such as release paper to form a functional ingredient layer, and then transferring the functional ingredient layer to a substrate; there is no particular limitation to the method used. EXAMPLES
[0092] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0093] Example 1 A side-by-side type latent crimped fiber (fiber diameter: 11.0 μm, fiber length: 44 mm, white, cross section: circular) made of a combination of polyester (melting point: 250 °C) and copolymer polyester (melting point: 230 °C) was used at 100 mass%, and the fiber was opened by a carding machine to form a parallel web (basis weight: 15 g / m) oriented in the warp direction. 2 ) was formed.
[0094] The parallel webs formed in the same manner as the above parallel webs were crossed in the vertical direction by a cross layer to form a cross web (basis weight: 15 g / m 2 ) was formed.
[0095] Next, the parallel web and the cross web are laminated to form a criss-cross web (basis weight: 30 g / m 2 ), and then using a single row nozzle (diameter: 0.13 mm, pitch: 0.6 mm), a shower was applied to one side of the criss-cross web under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., and then hydroentanglement was performed in which water was sprayed at a pressure of 3 MPa onto the showered surface and then at a pressure of 3 MPa onto the opposite surface of the showered surface to form a hydroentangled fiber web.
[0096] Next, the hydroentangled fiber web was dried and then heat-treated at a temperature of 150°C using a hot air dryer to induce crimping of the latent crimped fibers. When forming highly crimped fibers, the hydroentangled fiber web was shrunk (area shrinkage rate: 32%) to produce a nonwoven fabric (basis weight: 44 g / m2) made of highly crimped fibers. 2 , average fiber diameter: 11.0 μm).
[0097] The nonwoven fabric was then heated and pressed at a temperature of 120° C. and a pressure of 0.4 MPa to adjust the thickness, producing a substrate with a thickness of 0.41 mm.
[0098] Example 2 A side-by-side type latent crimped fiber (fiber diameter: 14.3 μm, fiber length: 51 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0099] In addition, a splittable fiber having a fiber cross-sectional arrangement as shown in FIG. 1 and consisting of polyester resin 1 and nylon resin 2, which was spun by a composite spinning method, was prepared. The splittable fiber had a fiber diameter of 16.7 μm and a fiber length of 51 mm (can be split to produce eight fine fibers (white) having a fiber diameter of 4.2 μm and consisting of polyester resin 1 with a substantially triangular cross-sectional shape, and eight fine fibers (white) having a fiber diameter of 4.2 μm and consisting of nylon resin 2 with an I-shaped cross-sectional shape).
[0100] Next, 80 mass% of side-by-side type latent crimped fiber and 20 mass% of splittable fiber were mixed and opened by a carding machine to obtain a parallel web (basis weight: 15 g / m) oriented in the warp direction. 2 ) was formed.
[0101] The parallel webs formed in the same manner as the above parallel webs were crossed in the vertical direction by a cross layer to form a cross web (basis weight: 15 g / m 2 ) was formed.
[0102] Next, the parallel web and the cross web are laminated to form a criss-cross web (basis weight: 30 g / m 2 ), and then using a single-row nozzle (diameter: 0.13 mm, pitch: 0.6 mm), a shower was applied to one side of the criss-cross web under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., and then hydroentanglement was performed in which water was sprayed at a pressure of 5 MPa onto the showered surface and then at a pressure of 5 MPa onto the opposite surface of the showered surface to form a hydroentangled fiber web containing fine fibers generated from the splittable fibers.
[0103] Next, the hydroentangled fiber web was dried and then heat-treated at a temperature of 165°C using a hot air dryer to express the crimp of the latent crimped fiber. When forming the highly crimped fiber, the hydroentangled fiber web was shrunk (area shrinkage rate: 46%) to produce a nonwoven fabric (basis weight: 56 g / m2) containing the highly crimped fiber and the fine fiber. 2 , average fiber diameter: 6.6 μm).
[0104] The nonwoven fabric was then heated and pressurized at a temperature of 120° C. and a pressure of 0.4 MPa to adjust the thickness, producing a substrate with a thickness of 0.23 mm. When the surface of this substrate was observed under an electron microscope, no splittable fibers were observed, and it was confirmed that most of the splittable fibers had split into fine fibers.
[0105] Example 3 A polyester fine fiber (white, cross-sectional shape: circular) with a fiber diameter of 2.4 μm and fiber length of 3 mm was prepared. In addition, a core-sheath type adhesive fiber (fiber diameter: 10.1 μm, fiber length: 3 mm, white, cross-sectional shape: circular) was prepared with a polyester (melting point: 250°C) as the core component and a copolymer polyester (melting point: 110°C) as the sheath component.
[0106] Next, a slurry was formed in which polyester fine fibers and core-sheath type adhesive fibers were dispersed in a mass ratio of 70:30. The slurry was then drawn up and heat-treated at a temperature of 110°C to bond the fibers together by the adhesion of the sheath component of the core-sheath type adhesive fibers, producing a wet-bonded fiber web (basis weight: 50 g / m 2 ) was formed.
[0107] Next, the wet-bonded fiber web was subjected to hydroentanglement by spraying a water stream at a pressure of 3 MPa on one side of the wet-bonded fiber web using a single-row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., and then spraying water at a pressure of 3 MPa on the showered surface and then on the opposite surface of the showered surface to produce a hydroentangled nonwoven fabric (basis weight: 50 g / m2) containing polyester fine fibers and core-sheath type adhesive fibers. 2 , average fiber diameter: 2.6 μm).
[0108] The hydroentangled nonwoven fabric was then heated and pressurized at a temperature of 100° C. and a pressure of 0.4 MPa to adjust the thickness, producing a substrate with a thickness of 0.30 mm.
[0109] Example 4 A side-by-side type latent crimped fiber (fiber diameter: 10.1 μm, fiber length: 10 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0110] We also prepared a core-sheath adhesive fiber (fiber diameter: 10.1 μm, fiber length: 3 mm, white, cross-sectional shape: circular) with polyester (melting point: 250°C) as the core component and copolymer polyester (melting point: 110°C) as the sheath component.
[0111] Next, a slurry was formed in which side-by-side type latent crimped fibers and core-sheath type adhesive fibers were dispersed in a mass ratio of 90:10. The slurry was then drawn up and heat-treated at a temperature of 110°C to bond the fibers together by the adhesion of the sheath component of the core-sheath type adhesive fibers, producing a wet-bonded fiber web (basis weight: 30 g / m 2 ) was formed.
[0112] Next, the wet-bonded fiber web was subjected to hydroentanglement by spraying a water stream at a pressure of 3 MPa on the showered surface and then at a pressure of 3 MPa on the opposite surface of the showered surface using a single-row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) at a nozzle height of 2 cm and a conveyor speed of 5 m / min, thereby forming a hydroentangled fiber web.
[0113] Next, the hydroentangled fiber web was dried and then heat-treated at a temperature of 160°C using a hot air dryer to induce crimping of the latent crimped fibers. When forming highly crimped fibers, the hydroentangled fiber web was shrunk (area shrinkage rate: 47%) to produce a nonwoven fabric (basis weight: 57 g / m2) containing highly crimped fibers and core-sheath type adhesive fibers. 2 , average fiber diameter: 10.1 μm).
[0114] The nonwoven fabric was then heated and pressed at a temperature of 100° C. and a pressure of 0.3 MPa to adjust the thickness, producing a substrate with a thickness of 0.40 mm.
[0115] Example 5 Polyester fine fibers (white, cross-sectional shape: circular) with a fiber diameter of 2.4 μm and fiber length of 3 mm were prepared.
[0116] We also prepared a core-sheath adhesive fiber (fiber diameter: 10.1 μm, fiber length: 3 mm, white, cross-sectional shape: circular) with polyester (melting point: 250°C) as the core component and copolymer polyester (melting point: 110°C) as the sheath component.
[0117] Furthermore, a side-by-side type latent crimped fiber (fiber diameter: 10.1 μm, fiber length: 10 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0118] First, a slurry was formed in which polyester fine fibers and core-sheath type adhesive fibers were dispersed in a mass ratio of 70:30. The slurry was then drawn up and heat-treated at a temperature of 110°C to bond the fibers together by the adhesion of the sheath component of the core-sheath type adhesive fibers, producing a wet-bonded fiber web (basis weight: 6 g / m 2 ) was formed to form a supporting nonwoven fabric.
[0119] Next, a slurry in which the latent crimped fibers are dispersed is formed, and this slurry is woven onto the supporting nonwoven fabric to form a fiber layer of the latent crimped fibers (basis weight: 24 g / m 2 ) was formed on a supporting nonwoven fabric.
[0120] Next, the support nonwoven fabric on which the fiber layer was formed was showered with a single-row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) at a nozzle height of 2 cm and a conveyor speed of 5 m / min., and then water was sprayed twice on the shower surface at pressures of 3 MPa and 5 MPa, and then once on the surface opposite the shower surface at a pressure of 5 MPa to perform hydroentanglement, thereby forming a hydroentangled laminated nonwoven fabric.
[0121] Next, the hydroentangled laminated nonwoven fabric was dried and then heat-treated at a temperature of 160°C using a hot air dryer to express the crimp of the latent crimped fibers and form highly crimped fibers. The hydroentangled laminated nonwoven fabric was then shrunk (area shrinkage rate: 47%) to form a two-layer laminated nonwoven fabric (basis weight: 57 g / m2) consisting of a nonwoven fabric layer mainly made of highly crimped fibers and a supporting nonwoven fabric layer containing polyester fine fibers and core-sheath type adhesive fibers. 2 , average fiber diameter: 4.3 μm).
[0122] The thickness of this two-layered nonwoven fabric was adjusted by heating and pressing it at a temperature of 100° C. and a pressure of 0.3 MPa to produce a substrate with a thickness of 0.39 mm.
[0123] Comparative Example 1 A random fiber web (basis weight: 40 g / m2) with randomly oriented fibers was produced by using 100 mass% side-by-side latent crimped fibers (fiber diameter: 14.3 μm, fiber length: 51 mm, white color, cross section: circular) made of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) and opening the fibers with a random carding machine. 2 ) was formed.
[0124] Next, the random fiber web was subjected to hydroentanglement by spraying water onto one side of the random fiber web using a single row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., followed by spraying water at a pressure of 4 MPa onto the showered surface and then spraying water at a pressure of 4 MPa onto the opposite side of the showered surface, thereby forming a hydroentangled fiber web.
[0125] Next, the hydroentangled fiber web is dried and then heat-treated at a temperature of 165°C using a hot air dryer to induce crimping of the latent crimped fibers. When forming highly crimped fibers, the hydroentangled fiber web is shrunk (area shrinkage rate: 50%) to produce a nonwoven fabric (basis weight: 80 g / m2) made of highly crimped fibers. 2 , average fiber diameter: 14.3 μm).
[0126] The nonwoven fabric was then heated and pressed at a temperature of 120° C. and a pressure of 0.4 MPa to adjust the thickness, producing a substrate with a thickness of 0.65 mm.
[0127] Comparative Example 2 In the same manner as in Comparative Example 1, the basis weight was 30 g / m 2 A random fiber web of 100 mm was formed.
[0128] Next, the hydroentangled fiber web formed by hydroentanglement under the same conditions as in Comparative Example 1 was dried, and then heat-treated at a temperature of 160°C using a hot air dryer to express the crimp of the latent crimped fiber and form highly crimped fibers. In this way, the hydroentangled fiber web was shrunk (area shrinkage rate: 46%) to produce a nonwoven fabric (basis weight: 56 g / m2) made of highly crimped fibers. 2 , average fiber diameter: 14.3 μm).
[0129] The nonwoven fabric was then heated and pressed at a temperature of 120° C. and a pressure of 0.3 MPa to adjust the thickness, producing a substrate with a thickness of 0.51 mm.
[0130] Example 6 A side-by-side type latent crimped fiber (fiber diameter: 11.0 μm, fiber length: 10 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0131] In addition, we prepared a core-sheath adhesive fiber (fiber diameter: 10.1 μm, fiber length: 5 mm, white, cross-sectional shape: circular) with polyester (melting point: 250°C) as the core component and copolymer polyester (melting point: 110°C) as the sheath component.
[0132] Next, a slurry was formed in which side-by-side type latent crimped fibers and core-sheath type adhesive fibers were dispersed in a mass ratio of 80:20. The slurry was then drawn up and heat-treated at a temperature of 110°C to bond the fibers together by the adhesion of the sheath component of the core-sheath type adhesive fibers, producing a wet-bonded fiber web (basis weight: 30 g / m 2 ) was formed.
[0133] Next, the wet-bonded fiber web is subjected to a heat treatment at a temperature of 160°C using a hot air dryer to develop the crimp of the latent crimp fiber, and when forming the highly crimped fiber, the wet-bonded fiber web is shrunk (area shrinkage rate: 41%, transverse shrinkage rate: 35%) to produce a nonwoven fabric (basis weight: 51 g / m2) containing the highly crimped fiber and the core-sheath type adhesive fiber. 2 , average fiber diameter: 10.8 μm).
[0134] The nonwoven fabric was then heated and pressed at a temperature of 100° C. and a pressure of 0.3 MPa to adjust the thickness, producing a substrate with a thickness of 0.39 mm.
[0135] Example 7 The basis weight of the wet-bonded fiber web is 20 g / m 2 A nonwoven fabric (basis weight: 54 g / m2) was prepared in the same manner as in Example 6, except that the area shrinkage rate of the wet-bonded fiber web was 63% and the transverse shrinkage rate was 60%. 2 After forming the fiber bundle (average fiber diameter: 10.8 μm), the thickness was adjusted by heating and pressurizing at a temperature of 100° C. and a pressure of 0.3 MPa to produce a substrate with a thickness of 0.40 mm.
[0136] Example 8 A side-by-side type latent crimped fiber (fiber diameter: 11.0 μm, fiber length: 10 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0137] We also prepared a core-sheath adhesive fiber (fiber diameter: 10.1 μm, fiber length: 3 mm, white, cross-sectional shape: circular) with polyester (melting point: 250°C) as the core component and copolymer polyester (melting point: 110°C) as the sheath component.
[0138] Next, a slurry was formed in which side-by-side type latent crimped fibers and core-sheath type adhesive fibers were dispersed in a mass ratio of 80:20. The slurry was then drawn up and heat-treated at a temperature of 110°C to bond the fibers together by the adhesion of the sheath component of the core-sheath type adhesive fibers, producing a wet-bonded fiber web (basis weight: 30 g / m 2 ) was formed.
[0139] Next, the wet-bonded fiber web was subjected to hydroentanglement by spraying a water stream at a pressure of 3 MPa on the showered surface and then at a pressure of 3 MPa on the opposite surface of the showered surface using a single-row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) at a nozzle height of 2 cm and a conveyor speed of 5 m / min, thereby forming a hydroentangled fiber web.
[0140] Next, the hydroentangled fiber web was dried and then heat-treated at a temperature of 170°C using a hot air dryer to induce crimping of the latent crimped fibers. When forming highly crimped fibers, the hydroentangled fiber web was shrunk (area shrinkage rate: 54%, transverse shrinkage rate: 46%) to produce a nonwoven fabric (basis weight: 65 g / m2) containing highly crimped fibers and core-sheath type adhesive fibers. 2 , average fiber diameter: 10.8 μm).
[0141] The nonwoven fabric was then heated and pressed at a temperature of 100° C. and a pressure of 0.3 MPa to adjust the thickness, producing a substrate with a thickness of 0.26 mm.
[0142] Example 9 A side-by-side type latent crimped fiber (fiber diameter: 14.3 μm, fiber length: 15 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0143] Next, a slurry in which the side-by-side type latent crimped fibers are dispersed is formed, and the slurry is drawn up and then dried at a temperature of 100°C to obtain a wet-laid fiber web (basis weight: 30 g / m 2 ) was formed.
[0144] Next, the wet fiber web was subjected to hydroentanglement by spraying water onto one side of the wet fiber web using a single row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., followed by spraying water at a pressure of 3 MPa onto the showered surface and then spraying water at a pressure of 3 MPa onto the opposite side of the showered surface, thereby forming a hydroentangled fiber web.
[0145] Next, the hydroentangled fiber web was subjected to a heat treatment at a temperature of 160°C using a hot air dryer to develop the crimp of the latent crimped fiber, and when forming highly crimped fibers, the hydroentangled fiber web was shrunk (area shrinkage rate: 46%) to produce a nonwoven fabric (basis weight: 55 g / m2) made of highly crimped fibers. 2 , average fiber diameter: 14.3 μm).
[0146] The nonwoven fabric was then heated and pressed at a temperature of 130° C. and a pressure of 0.4 MPa to adjust the thickness, producing a substrate with a thickness of 0.20 mm.
[0147] Example 10 A side-by-side type latent crimped fiber (fiber diameter: 14.3 μm, fiber length: 15 mm, white, cross-sectional shape: circular) consisting of a combination of polyester (melting point: 250°C) and copolymer polyester (melting point: 230°C) was prepared.
[0148] Next, a slurry in which the side-by-side type latent crimped fibers are dispersed is formed, and the slurry is drawn up and then dried at a temperature of 100°C to obtain a wet-laid fiber web (basis weight: 30 g / m 2 ) was formed.
[0149] Next, the wet fiber web was subjected to hydroentanglement by spraying water onto one side of the wet fiber web using a single row nozzle (diameter: 0.13 mm, pitch: 0.6 mm) under conditions of a nozzle height of 2 cm and a conveyor speed of 5 m / min., followed by spraying water at a pressure of 3 MPa onto the showered surface and then spraying water at a pressure of 3 MPa onto the opposite side of the showered surface, thereby forming a hydroentangled fiber web.
[0150] Next, the hydroentangled fiber web was subjected to a heat treatment at a temperature of 160°C using a hot air dryer to develop the crimp of the latent crimped fiber, and when forming highly crimped fibers, the hydroentangled fiber web was shrunk (area shrinkage rate: 58%) to produce a nonwoven fabric (basis weight: 71 g / m2) made of highly crimped fibers. 2 , average fiber diameter: 14.3 μm).
[0151] The nonwoven fabric was then heated and pressed at a temperature of 130° C. and a pressure of 0.3 MPa to adjust the thickness, producing a substrate with a thickness of 0.43 mm.
[0152] (Substrate evaluation) For the substrates of Examples 1 to 10 and Comparative Examples 1 and 2, the basis weight, thickness, surface dynamic friction coefficient, tensile strength, elongation, tensile strength at 20% elongation, tensile strength at 50% elongation, recovery rate at 20% elongation, recovery rate at 50% elongation, air permeability, unit thickness air permeability, and thickness air permeability constant were evaluated by the methods described above.
[0153] The maximum dynamic friction coefficient, peel resistance, and exudation resistance of the functional components of the substrate were evaluated by the following methods.
[0154] (Maximum dynamic friction coefficient) A film-like polystyrene adhesive (thickness: 50 μm) with a polyester separator was placed on each substrate and bonded at a temperature of 90°C and a pressure of 0.01 MPa. The substrates were then cut into rectangles measuring 2 cm x 4 cm, and three rectangular test pieces were taken from each substrate.
[0155] After cleaning the sample stage (made of stainless steel) of a static and dynamic friction tester (manufactured by Trinity Lab Co., Ltd., product number: TL201Tt) with ethanol, the polyester separator was peeled off from the test piece, and the test piece was attached to the sample stage with a polystyrene-based adhesive.
[0156] Next, cotton No. 3-1 specified in JIS L 0803 was attached to the contact terminal (area: 1 cm) of the static and dynamic friction measuring instrument. 2 ) and the contact terminal was set approximately 1 cm away from the end of the long side of the test piece.
[0157] Then, while applying a load of 100 g (N = normal force) to the contact terminal, the dynamic friction force (F) was measured at a speed of 10 mm / sec. and a scanning distance of 4 cm (= scanning only 3 cm from the end of the long side of the test piece).
[0158] At this time, the following relationship generally holds between the kinetic friction force (F), normal force (N), and kinetic friction coefficient (μ') when the contact terminal hits the long side end of the test piece, so the value of the kinetic friction coefficient (μ') was calculated using the following formula. F=μ'N μ'=F / N
[0159] The dynamic friction coefficient was measured for each of three test pieces taken from each substrate, and the arithmetic mean value was taken as the maximum dynamic friction coefficient.
[0160] When the patch is used, it is likely to peel off from the edge due to rubbing against clothing, etc., so the maximum dynamic friction coefficient serves as an index of how easily the patch will peel off due to rubbing against clothing, etc. A large maximum dynamic friction coefficient means that the patch will peel off easily due to the action of a large external force.
[0161] (Difficulty in peeling) A film-like polystyrene adhesive (thickness: 50 μm) with a polyester separator was placed on each substrate and bonded at a temperature of 90°C and a pressure of 0.01 MPa. The substrates were then cut into rectangles measuring 2 cm x 4 cm, and three rectangular test pieces were taken from each substrate.
[0162] After cleaning the sample stage (made of stainless steel) of a static and dynamic friction tester (manufactured by Trinity Lab Co., Ltd., product number: TL201Tt) with ethanol, the polyester separator was peeled off from the test piece, and the test piece was attached to the sample stage with a polystyrene-based adhesive.
[0163] Next, cotton No. 3-1 specified in JIS L 0803 was attached to the contact terminal (area: 1 cm) of the static and dynamic friction measuring instrument. 2 ) and the contact terminal was set approximately 1 cm away from the end of the long side of the test piece.
[0164] Then, with a load of 100 g applied to the contact terminal, the test piece was scanned 10 times at a speed of 10 mm / sec. and a scanning distance of 4 cm (=scanning only 3 cm from the end of the long side of the test piece), and the degree of peeling of the test piece from the sample stand was then numerically evaluated according to the following criteria.
[0165] The degree of peeling was evaluated numerically for each of the three test pieces taken from each substrate, and the resistance to peeling was evaluated based on the arithmetic mean value according to the following criteria.
[0166] Note (Degree of peeling) 5 points: The test piece has not come off the sample base at all. 3 points: Part of the edge of the test piece was peeled off from the sample stand. 1 point: The entire edge of the test piece or the entire test piece was peeled off from the sample base.
[0167] (Difficulty in peeling) 〇: 11 points or more △:5~11 points ×: 5 points or less
[0168] (Hardness of functional ingredients seeping out) Each substrate was cut into a 5cm x 20cm rectangle to obtain three test pieces. On the other hand, a film-like polystyrene adhesive (thickness: 50μm) with a polyester separator was cut into a 2cm x 15cm rectangle, and the adhesive with separator was laminated to the center of the test piece so that the long sides of the substrate and the adhesive with separator were parallel, and the test piece was heated and pressurized at a temperature of 110℃ and a pressure of 0.4MPa to adhere the adhesive with separator to the test piece, preparing a laminated test piece.
[0169] Next, the laminated test piece was cut in the short side direction at the center of the long side direction of the laminated test piece to obtain two laminated test pieces, and then the laminated test pieces were stacked so that the substrate sides of the laminated test pieces were in contact with each other, and heated and pressed at a temperature of 110°C and a pressure of 0.4 MPa.
[0170] Thereafter, the two laminated test pieces were peeled off, and the resistance to bleeding of the functional ingredients was evaluated numerically according to the following criteria.
[0171] This numerical evaluation of the resistance to bleeding was carried out for each of the three laminated test pieces prepared by taking samples from each substrate, and the resistance to bleeding was evaluated based on the arithmetic mean value according to the following criteria.
[0172] Note (degree of seepage) 5 points: No adhesion at all 3 points: Some parts are sticky 1 point: The entire surface is adhesive
[0173] (Difficulty in peeling) 〇: 11 points or more △:5~11 points ×: 5 points or less
[0174] The evaluation results of the substrates of Examples 1 to 10 and Comparative Examples 1 and 2 are shown in Tables 1 to 3.
[0175] [Table 1]
[0176] [Table 2]
[0177] [Table 3]
[0178] Comparing the Examples and Comparative Examples, it was found that when the thickness was 0.48 mm or less, the maximum dynamic friction coefficient was small and the substrate was less likely to peel off. In addition, it was found that when the unit thickness air permeability was less than 431, the substrate was less likely to exude functional ingredients.
[0179] It was also found that by having a thickness air permeability constant of less than 109, preferably 100 or less, the substrate is one through which the functional component is less likely to seep out.
[0180] Furthermore, it was found that when fine fibers were included as in Examples 2, 3, and 5, the thickness of the substrate could be made thinner, making the substrate less susceptible to peeling.
[0181] Furthermore, the substrates of Examples 6 to 8 had low tensile strength at 50% elongation in the horizontal direction and were therefore easily stretched, and therefore had excellent adhesion to objects that require large elongation, such as elbows and knees, and could be used to produce patches that were also comfortable to wear.
[0182] The substrates of Examples 9 and 10 had low tensile strength at 20% elongation and 50% elongation in both the vertical and horizontal directions, and had good stretchability in both directions. Therefore, these substrates could provide a good application feeling regardless of the shape of the patch or the application direction. [Industrial Applicability]
[0183] The patch of the present invention can be, for example, a patch intended to exert an anti-inflammatory and analgesic effect, an objective to exert a cosmetic effect by a cosmetic agent, or an objective to give a warm or cool sensation, and the patch base material can be the base material of these patches. For example, the patch of the present invention can be a cataplasm, a plaster, a tape preparation, a surgical tape, a taping material or a bandage, a facial mask, a warming sheet or a cooling sheet, and the patch base material of the present invention can be the base material of these patches. [Explanation of symbols]
[0184] 1. Polyester resin 2. Nylon resin
Claims
1. A patch base material having a fiber sheet and a thickness of 0.48 mm or less, the fiber sheet being a fiber sheet containing highly crimped fibers in which crimping of latent crimped fibers has been expressed (excluding nonwoven fabrics having an elongation rate of 100% or more in both the warp and weft directions), or a fiber sheet containing a wet-laid nonwoven fabric containing fine fibers having a fiber diameter of 6 μm or less, and further satisfying the following formula: Note 0<(breathability of patch base material / thickness of patch base material)<431
2. A patch comprising the patch base material according to claim 1.
Citation Information
Patent Citations
Plaster base fabric for medical application and its production
JP1999012910A
Base fabric for medicinal cataplasm
JP2000143504A
Porous sheet
JP2001248057A
Medical adhesive tape base material and its manufacturing method
JP2007075502A