Electrophotographic photoreceptor, process cartridge, and image forming apparatus

The electrophotographic photoreceptor stabilizes charge transport ability and prevents potential rise by using a fluorine-containing resin layer with a dispersant and strategically arranged charge transport materials, addressing fluctuations caused by discharge products.

JP7593193B2Active Publication Date: 2024-12-03FUJIFILM BUSINESS INNOVATION CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021054289
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-12-03
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing electrophotographic photoreceptors experience fluctuations in charge transport ability and increased potential after prolonged use due to discharge products, which are not effectively addressed by current technologies.

Method used

The photoreceptor incorporates a fluorine-containing resin layer with a dispersant and multiple charge transport materials arranged by descending HOMO energy levels, maintaining a specific energy level difference and content ratio to stabilize charge transport capacity.

Benefits of technology

This configuration suppresses fluctuations in charge transport ability and prevents potential increases over time, ensuring stable performance of the photoreceptor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593193000018
    Figure 0007593193000018
  • Figure 0007593193000019
    Figure 0007593193000019
  • Figure 0007593193000020
    Figure 0007593193000020
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor that can prevent a variation in charge transport ability caused by a discharge product and can prevent an increase in potential after exposure when used for a long period.SOLUTION: An electrophotographic photoreceptor has a conductive substrate and a photosensitive layer provided on the conductive substrate. An outermost surface layer includes fluorine-containing resin particles, fluorine-containing dispersant, and two or more types of charge transport materials. When the two or more types of charge transport materials are arranged in descending order from the highest HOMO energy level, the HOMO energy level difference between the adjacent charge transfer materials exceeds 0 eV and 0.2 eV or less. The ratio A of the content of the charge transport materials to the total amount of the two or more types of charge transport materials satisfies the condition 1: [(100 / N)-(100 / N×0.3)]≤A≤[(100 / N)+(100 / N×0.3)] (N is the number of types of the charge transport materials included in the outermost surface layer).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, a process cartridge, and an image forming apparatus. [Background technology]

[0002] Patent Document 1 discloses an electrophotographic photoreceptor having, as the outermost layer, a charge transport layer containing two types of charge transport materials. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6447200 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide an electrophotographic photoreceptor which has an outermost surface layer containing fluorine-containing resin particles, a fluorine-containing dispersant, and two or more charge transport materials, and which can suppress fluctuations in charge transport ability caused by discharge products and can suppress potential rise after exposure when used for a long period of time, compared to a case in which the difference in HOMO energy levels between adjacent charge transport materials exceeds 0.2 eV when the two or more charge transport materials are arranged in order from highest to lowest HOMO energy level, or a case in which the ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials does not satisfy the above-mentioned condition 1. [Means for solving the problem]

[0005] Specific means for solving the above problems include the following aspects.

[0006] <1> A conductive substrate and a photosensitive layer provided on the conductive substrate, the outermost layer contains fluorine-containing resin particles, a fluorine-containing dispersant, and two or more kinds of charge transport materials; When the two or more charge transport materials are arranged in order from the highest HOMO energy level to the lowest, the difference in HOMO energy levels between adjacent charge transport materials is greater than 0 eV and less than or equal to 0.2 eV, and The electrophotographic photoreceptor has a ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials, which satisfies the following condition 1: Condition 1: [(100 / N)-(100 / N×0.3)]≦A≦[(100 / N)+(100 / N×0.3)] (In condition 1, N represents the number of types of charge transport materials contained in the outermost layer.)

[0007] <2> When the two or more charge transport materials are arranged in order from the highest HOMO energy level, the difference in HOMO energy levels between adjacent charge transport materials is 0.01 eV or more and 0.2 eV or less. <1> The electrophotographic photoreceptor according to claim 1. <3> The activation energy is 0.35 eV or less. <2> The electrophotographic photoreceptor according to claim 1. <4> The ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials satisfies the following condition 2: <1> ~ <3> 13. The electrophotographic photoreceptor according to claim 12, Condition 2: [(100 / N)-(100 / N×0.2)]≦A≦[(100 / N)+(100 / N×0.2)] (In condition 2, N represents the number of types of charge transport materials contained in the outermost layer.)

[0008] <5> The number of carboxyl groups in the fluorine-containing resin particles is 10 6 Between 0 and 30 pieces per piece, <1> ~ <4> 13. The electrophotographic photoreceptor according to claim 12, <6> The content of the fluorine-containing dispersant is 0.25% by mass or more and 0.4% by mass or less with respect to the total mass of the outermost surface layer. <1> ~ <5> The electrophotographic photoreceptor according to claim 1. <7> The two or more kinds of charge transport materials are contained in an amount of 30% by mass or more and 60% by mass or less based on the total mass of the outermost layer. <1> ~ <6> 13. The electrophotographic photoreceptor according to claim 12,

[0009] <8> The two or more charge transport materials include a compound represented by the following formula (CT1): <7> The electrophotographic photoreceptor according to claim 1.

[0010] [ka]

[0011] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 20 carbon atoms, an alkoxy group having from 1 to 20 carbon atoms, or an aryl group having from 6 to 30 carbon atoms, and two adjacent substituents may be bonded to each other to form a hydrocarbon ring structure. each independently represents 0, 1, or 2.

[0012] <9> The two or more charge transport materials include a compound represented by the following formula (CT2): <7> or <8> The electrophotographic photoreceptor according to claim 1.

[0013] [ka]

[0014] In formula (CT2), R C21 , R C22 , and R C23 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, an alkyl group, an alkoxy group, or an aryl group.

[0015] <10> <1> ~ <9> The electrophotographic photoreceptor according to any one of the above items is provided, A process cartridge that is detachably attached to an image forming apparatus. <11> <1> ~ <9> and an electrophotographic photoreceptor according to any one of the above items. a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising: Effect of the Invention

[0016] <1> or <2> According to the invention described in the above, there is provided an electrophotographic photoreceptor which has an outermost surface layer containing fluorine-containing resin particles, a fluorine-containing dispersant, and two or more charge transport materials, and which can suppress fluctuations in charge transport ability caused by discharge products and can suppress potential rise after exposure during long-term use, as compared with a case in which the difference in HOMO energy levels between adjacent charge transport materials exceeds 0.2 eV when the two or more charge transport materials are arranged in order from the highest HOMO energy level, or a case in which the ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials does not satisfy the above condition 1.

[0017] <3> According to the present invention, there is provided an electrophotographic photoreceptor which can suppress fluctuations in charge transport ability caused by discharge products and can suppress an increase in potential after exposure when used for a long period of time, as compared with a case in which the activation energy exceeds 0.35 eV. <4> According to the invention, there is provided an electrophotographic photoreceptor which can suppress fluctuations in charge transport ability caused by discharge products and can suppress an increase in potential after exposure during long-term use, as compared with a case in which the content ratio A of each charge transport material does not satisfy the above-mentioned condition 2. <5> According to the present invention, the number of carboxyl groups in the fluorine-containing resin particles is 10 6 As compared with the case where the number of particles per particle is more than 30, an electrophotographic photoreceptor having excellent charging properties is provided. <6> According to the present invention, there is provided an electrophotographic photoreceptor which can suppress a rise in potential after exposure during long-term use, as compared with a case in which the content of the fluorine-containing dispersant exceeds 0.4 mass % relative to the total mass of the outermost layer. <7> According to the present invention, an electrophotographic photoreceptor having excellent charge transporting ability is provided, as compared with a case where the amount of two or more charge transporting materials is less than 30% by mass or more than 60% by mass based on the total mass of the outermost layer.

[0018] <8> or <9> According to the present invention, an electrophotographic photoreceptor having excellent charge transport properties is provided, as compared with a case in which the two or more charge transport materials do not contain a compound represented by formula (CT1) or formula (CT2).

[0019] <10> or <11> According to the invention, there is provided a process cartridge or an image forming apparatus equipped with an electrophotographic photoreceptor which has an outermost surface layer containing fluorine-containing resin particles, a fluorine-containing dispersant, and two or more charge transport materials, and which is capable of suppressing fluctuations in charge transport ability caused by discharge products and suppressing potential rise after exposure during long-term use, compared to a case in which the difference in HOMO energy levels between adjacent charge transport materials exceeds 0.2 eV when the two or more charge transport materials are arranged in order from highest to lowest HOMO energy level, or a case in which the ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials does not satisfy condition 1. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of a layer structure of the electrophotographic photoreceptor according to the present embodiment. [Diagram 2] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic configuration diagram illustrating another example of an image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, embodiments of the present invention will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0022] In the numerical ranges described in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in another stepwise manner. In addition, in the numerical ranges described in this disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0023] In this specification, each component may contain multiple corresponding substances. In this specification, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.

[0024] <Electrophotographic photoreceptor> The electrophotographic photoreceptor according to the present embodiment has a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost layer contains fluorine-containing resin particles, a fluorine-containing dispersant, and two or more charge transport materials, and when the two or more charge transport materials are arranged in order from highest to lowest HOMO energy level, the HOMO energy level difference between adjacent charge transport materials is more than 0 eV and not more than 0.2 eV, and the ratio A of the content of each charge transport material to the total amount of the two or more charge transport materials satisfies the following condition 1: Condition 1: [(100 / N)-(100 / N×0.3)]≦A≦[(100 / N)+(100 / N×0.3)] (In condition 1, N represents the number of types of charge transport materials contained in the outermost layer.)

[0025] In electrophotographic photoreceptors, the discharge products react with the charge transport material contained in the outermost layer, and the charge transport material is oxidized, which may cause local variations in the charge transport ability on the surface. In addition, when the electrophotographic photoreceptor is used for a long period of time, the dispersant of the particles contained in the outermost layer may cause accumulation of charges, resulting in an increase in the potential after exposure. The electrophotographic photoreceptor according to the present embodiment has the above-mentioned configuration, and therefore can suppress the fluctuation of the charge transport ability caused by the discharge products and the increase in potential after exposure during long-term use. Although the reason for this is not necessarily clear, it can be assumed as follows.

[0026] The electrophotographic photoreceptor according to the present embodiment uses two or more charge transport materials in the outermost layer, which have close but different HOMO energy levels. This allows the charge transport materials to have an energy state in which oxidation of the charge transport materials by discharge products is unlikely to occur due to the interaction between the charge transport materials, and it is presumed that even if some of the charge transport materials are oxidized, the other charge transport materials compensate for the charge transport ability, thereby suppressing the fluctuation of the charge transport ability. In addition, even if the outermost surface layer contains a fluorine-containing dispersant, it is presumed that by further containing two or more charge transport materials having similar but different HOMO energy levels, even if charge accumulation occurs during long-term use of the electrophotographic photoreceptor, the accumulated charge is easily released, and an increase in potential after exposure is suppressed.

[0027] <Layer structure of electrophotographic photoreceptor> Hereinafter, the layer structure of the electrophotographic photoreceptor will be described with reference to the drawings. 1 has a structure in which, for example, an undercoat layer 1, a charge generation layer 2, and a charge transport layer 3 are laminated in this order on a conductive support 4. The charge generation layer 2 and the charge transport layer 3 constitute a photosensitive layer 5. In this case, the charge transport layer 3 constitutes the outermost layer.

[0028] The electrophotographic photoreceptor according to the present embodiment may have a layer structure in which the undercoat layer 1 is not provided. The electrophotographic photoreceptor according to the present embodiment may be a photoreceptor having a single-layer type photosensitive layer in which the functions of the charge generating layer 2 and the charge transport layer 3 are integrated. In the case of a photoreceptor having a single-layer type photosensitive layer, the single-layer type photosensitive layer constitutes the outermost layer. The electrophotographic photoreceptor according to the present embodiment may be a photoreceptor having a surface protective layer on the charge transport layer 3 or on the single-layer type photoreceptor. In the case of a photoreceptor having a surface protective layer, the surface protective layer constitutes the outermost surface layer. That is, in the electrophotographic photoreceptor according to the present embodiment, the outermost layer corresponds to the charge transport layer, the single-layer type photosensitive layer, or the surface protective layer, as described above.

[0029] Each layer of the electrophotographic photoreceptor according to this embodiment will be described in detail below, with the reference numerals shown in FIG.

[0030] ≪Top surface layer≫ In the electrophotographic photoreceptor according to this embodiment, the outermost layer contains fluorine-containing resin particles, a fluorine-containing dispersant, and two or more kinds of charge transport materials. The fluorine-containing resin particles, the fluorine-containing dispersant, and the two or more kinds of charge transport materials contained in the outermost layer will be described in detail below.

[0031] The outermost layer may contain other components in addition to the fluorine-containing resin particles, the fluorine-containing dispersant, and the two or more kinds of charge transport materials depending on the type of layer (i.e., charge transport layer, single-layer type photosensitive layer, or surface protective layer). The other components will be described in the section for each corresponding layer (i.e., charge transport layer, single-layer type photosensitive layer, or surface protective layer).

[0032] [Fluorine-containing resin particles] The outermost layer contains fluorine-containing resin particles. The fluorine-containing resin particles may be used alone or in combination of two or more kinds.

[0033] Fluorine-containing resin Examples of the fluorine-containing resin that constitutes the fluorine-containing resin particles include (1) particles of a homopolymer of a fluoroolefin, and (2) a copolymer of two or more types of fluoroolefins, which is a copolymer of one or more types of fluoroolefins and a non-fluorine-based monomer (i.e., a monomer that does not have a fluorine atom).

[0034] Examples of the fluoroolefin include perhaloolefins such as tetrafluoroethylene (TFE), perfluorovinyl ether, hexafluoropropylene (HFP), and chlorotrifluoroethylene (CTFE), and non-perfluoroolefins such as vinylidene fluoride (VdF), trifluoroethylene, and vinyl fluoride. Among these, the fluoroolefin preferably includes one or more selected from the group consisting of VdF, TFE, CTFE, and HFP.

[0035] Examples of non-fluorine-based monomers include hydrocarbon olefins such as ethylene, propylene, and butene; alkyl vinyl ethers such as cyclohexyl vinyl ether (CHVE), ethyl vinyl ether (EVE), butyl vinyl ether, and methyl vinyl ether; alkenyl vinyl ethers such as polyoxyethylene allyl ether (POEAE) and ethyl allyl ether; organic silicon compounds having reactive α,β-unsaturated groups such as vinyltrimethoxysilane (VSi), vinyltriethoxysilane, and vinyltris(methoxyethoxy)silane; acrylic acid esters such as methyl acrylate and ethyl acrylate; methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; vinyl esters such as vinyl acetate, vinyl benzoate, and "Veova" (trade name, vinyl ester manufactured by Shell); and the like. Among these, the non-fluorine-based monomer preferably contains at least one selected from the group consisting of alkyl vinyl ethers, allyl vinyl ethers, vinyl esters, and organic silicon compounds having reactive α,β-unsaturated groups.

[0036] Among these, the fluorine-containing resin preferably contains a resin with a high fluorination rate, more preferably contains one or more resins selected from the group consisting of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), and ethylene-chlorotrifluoroethylene copolymer (ECTFE), and even more preferably contains one or more resins selected from the group consisting of PTFE, FEP, and PFA.

[0037] - Method for granulating fluorine-containing resin The method for forming particles of the fluorine-containing resin is not particularly limited, and may be any of a method of forming particles by irradiation with radiation (in this specification, particles obtained by this method are also referred to as "radiation-irradiated fluorine-containing resin particles"), a method of forming particles by polymerization (in this specification, particles obtained by this method are also referred to as "polymerization-type fluorine-containing resin particles"), and the like.

[0038] The term "radiation-exposed fluorine-containing resin particles (fluorine-containing resin particles obtained by irradiation with radiation)" refers to fluorine-containing resin particles that are granulated during radiation polymerization and that are reduced in molecular weight and atomized by irradiation of the fluorine-containing resin after polymerization. Radiation-exposed fluorine-containing resin particles also contain a large amount of carboxyl groups because a large amount of carboxylic acid is produced by irradiation in air.

[0039] Polymerized fluorine-containing resin particles (fluorine-containing resin particles obtained by polymerization) refer to fluorine-containing resin particles that are granulated during polymerization by a suspension polymerization method, an emulsion polymerization method, etc., and that are not irradiated with radiation. Polymerized fluorine-containing resin particles are produced by polymerization in the presence of a basic compound, and therefore contain the basic compound as a residue.

[0040] Among these, the fluorine-containing resin particles are preferably polymerized fluorine-containing resin particles, which are granulated during polymerization by a suspension polymerization method, an emulsion polymerization method or the like without irradiation with radiation, as described above. The production of fluorine-containing resin particles by the suspension polymerization method is, for example, a method in which additives such as a polymerization initiator, a catalyst, etc. are suspended in a dispersion medium together with a monomer for forming a fluorine-containing resin, and then the monomer is polymerized while the polymer is granulated. The production of fluorine-containing resin particles by emulsion polymerization is a method in which, for example, additives such as a polymerization initiator, a catalyst, and the like are emulsified in a dispersion medium together with a monomer for forming a fluorine-containing resin using a surfactant (i.e., an emulsifier), and then the monomer is polymerized while the polymerized product is granulated.

[0041] Carboxylic group The fluorine-containing resin particles preferably do not contain a carboxyl group, or if they do, the amount is small. Specifically, the number of carboxyl groups in the fluorine-containing resin particles is preferably 10 to 100 carbon atoms, from the viewpoint of providing an electrophotographic photoreceptor with excellent charging properties. 6 The number per unit is preferably 0 to 30, and more preferably 0 to 20.

[0042] Here, the carboxy group of the fluorine-containing resin particle refers to a carboxy group derived from a terminal carboxylic acid contained in the fluorine-containing resin particle.

[0043] The method for reducing the amount of carboxy groups in the fluorine-containing resin particles is not particularly limited, and examples thereof include (1) a method in which radiation is not irradiated during the process of forming the fluorine-containing resin into particles, and (2) a method in which radiation is irradiated under conditions in which oxygen is not present or under conditions in which the oxygen concentration is reduced.

[0044] The amount of carboxy groups in the fluorine-containing resin particles is measured as follows. -Pretreatment- When measuring the amount of carboxyl groups of the fluorine-containing resin particles in the outermost surface layer, the outermost surface layer is immersed in a solvent (e.g., tetrahydrofuran) to dissolve the fluorine-containing resin particles and substances insoluble in the solvent (here, tetrahydrofuran), and then the solution is dropped into pure water to filter out the precipitate. The insoluble matter obtained by filtration is further dissolved in the solvent, and then the solution is dropped into pure water to filter out the precipitate. This process is repeated five times, and the fluorine-containing resin particles are taken out and used as the measurement sample.

[0045] -measurement- The amount of carboxy groups in the fluorine-containing resin particles is measured as described in JP-A-4-20507. The fluorine-containing resin particles are preformed in a press to produce a film of approximately 0.1 mm thickness. The infrared absorption spectrum of the produced film is measured. The fluorine-containing resin particles are brought into contact with fluorine gas to produce fluorine-containing resin particles in which the carboxylic acid terminals are completely fluorinated. The infrared absorption spectrum is also measured, and the number of terminal carboxyl groups (10 carbon atoms) is calculated from the difference spectrum between the two, using the following formula: 6 (per piece).

[0046] Number of terminal carboxyl groups (10 carbon atoms) 6 per piece) = (l × K) / t l: Absorbance K: correction coefficient, t: film thickness (mm) The absorption wave number of the carboxyl group is 3560 cm -1 , the correction coefficient is 440.

[0047] Perfluorooctanoic acid From the viewpoint of improving electrostatic chargeability, it is preferable that the fluorine-containing resin particles do not contain perfluorooctanoic acid (also known as PFOA), or if they contain any, the amount is small. Specifically, the amount of PFOA in the fluorine-containing resin particles is preferably 0 ppb or more and 25 ppb or less, more preferably 0 ppb or more and 20 ppb or less, and more preferably 0 ppb or more and 15 ppb or less, based on the mass of the fluorine-containing resin particles.

[0048] PFOA is used or produced as a by-product during the production process of fluorine-containing resin particles (especially fluorine-containing resin particles such as polytetrafluoroethylene particles, modified polytetrafluoroethylene particles, and perfluoroalkyl ether / tetrafluoroethylene copolymer particles), and therefore the fluorine-containing resin particles often contain PFOA. In addition, since PFOA has a carboxy group that causes a decrease in the electrostatic charge of the particles, from the viewpoint of improving electrostatic charge, it is preferable that the fluorine-containing resin particles do not contain PFOA, or if they contain it, it is in a very small amount.

[0049] Methods for reducing the amount of PFOA include thoroughly washing fluorine-containing resin particles with pure water, alkaline water, alcohols (methanol, ethanol, isopropanol, etc.), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), esters (ethyl acetate, etc.), other common organic solvents (toluene, tetrahydrofuran, etc.), etc. Washing may be performed at room temperature, but it can be reduced more efficiently by performing it under heating.

[0050] The amount of PFOA contained in the fluorine-containing resin particles is a value measured by the following method. -Pretreatment- When measuring the amount of PFOA in the fluorine-containing resin particles contained in the outermost surface layer, the outermost surface layer is immersed in a solvent (e.g., tetrahydrofuran) and all substances other than the fluorine-containing resin particles and substances insoluble in the solvent are dissolved in the solvent (here, tetrahydrofuran), then the solution is dropped into pure water and the precipitate is filtered off. The solution containing PFOA obtained at this time is collected. The insoluble matter obtained by filtration is further dissolved in a solvent, and the solution is dropped into pure water and the precipitate is filtered off. This process is repeated five times, and the solution containing PFOA collected in the entire process is called the pretreated solution.

[0051] -measurement- Using the pretreated solution obtained by the above method, prepare a sample solution and measure the amount of PFOA according to the method shown in "Analysis of Perfluorooctane Sulfone Acid (PFOS) and Perfluorooctane Acid (PFOA) in Environmental Water, Sediment, and Organisms, Iwate Prefectural Environmental and Health Research Center."

[0052] Basic compounds It is preferable that the fluorine-containing resin particles do not contain a basic compound, or if they do, the amount is small. Specifically, the amount of the basic compound in the fluorine-containing resin particles is preferably 0 ppm or more and 3 ppm or less, more preferably 0 ppm or more and 1.5 ppm or less, and even more preferably 0 ppm or more and 1.2 ppm or less, from the viewpoint of obtaining an electrophotographic photoreceptor having excellent charging properties. Here, ppm is based on mass.

[0053] Specific examples of the basic compound contained in the fluorine-containing resin particles include 1) a basic compound derived from a polymerization initiator used when forming the fluorine-containing resin particles into particles during polymerization, 2) a basic compound used in the step of aggregating the particles after polymerization, and 3) a basic compound used as a dispersion aid for stabilizing the dispersion after polymerization.

[0054] Examples of basic compounds include amine compounds; hydroxides of alkali metals or alkaline earth metals; oxides of alkali metals or alkaline earth metals; acetates, etc. (e.g., particularly amine compounds); and the like. The basic compound is, for example, a basic compound having a boiling point (boiling point under normal pressure (1 atmosphere)) of 40°C or higher and 130°C or lower (preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 90°C or lower).

[0055] Examples of the amine compound include a primary amine compound, a secondary amine compound, and a tertiary amine compound.

[0056] Examples of the primary amine compound include methylamine, ethylamine, propylamine, isopropylamine, n-butylamine, isobutylamine, t-butylamine, hexylamine, 2-ethylhexylamine, secondary butylamine, allylamine, and methylhexylamine.

[0057] Examples of secondary amine compounds include dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-t-butylamine, dihexylamine, di(2-ethylhexyl)amine, N-isopropyl-N-isobutylamine, di(2-ethylhexyl)amine, di-secondary butylamine, diallylamine, N-methylhexylamine, 3-pipecoline, 4-pipecoline, 2,4-lupetidine, 2,6-lupetidine, 3,5-lupetidine, morpholine, and N-methylbenzylamine.

[0058] Tertiary amine compounds include trimethylamine, triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, triisobutylamine, tri-t-butylamine, trihexylamine, tri(2-ethylhexyl)amine, N-methylmorpholine, N,N-dimethylallylamine, N-methyldiallylamine, triallylamine, N,N-dimethylallylamine, N,N,N',N'-tetramethyl-1,2-diaminoethane, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N',N'-tetraallyl-1,4-diaminobutane, and N-methylpiperidine. , pyridine, 4-ethylpyridine, N-propyl diallylamine, 3-dimethylaminopropanol, 2-ethylpyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2,4-lutidine, 2,5-lutidine, 3,4-lutidine, 3,5-lutidine, 2,4,6-collidine, 2-methyl-4-ethylpyridine, 2-methyl-5-ethylpyridine, N,N,N',N'-tetramethylhexamethylenediamine, N-ethyl-3-hydroxypiperidine, 3-methyl-4-ethylpyridine, 3-ethyl-4-methylpyridine, 4-(5-nonyl)pyridine, imidazole, N-methylpiperazine, and the like.

[0059] Examples of hydroxides of alkali metals or alkaline earth metals include NaOH, KOH, Ca(OH)2, Mg(OH)2, Ba(OH)2, and the like. Examples of the oxides of alkali metals or alkaline earth metals include CaO and MgO. The acetates include zinc acetate and sodium acetate.

[0060] The method for reducing the amount of basic compounds contained in the fluorine-containing resin particles is not particularly limited, and examples thereof include: (1) a method in which, after the production of the particles, the particles are washed with water, an organic solvent (alcohols such as methanol, ethanol, isopropanol, and tetrahydrofuran, etc.); and (2) a method in which, after the production of the particles, the particles are heated (for example, heated to 200° C. or higher and 250° C. or lower) to decompose or vaporize and remove the basic compounds.

[0061] The amount of the basic compound contained in the fluorine-containing resin particles is measured as follows. -Pretreatment- When measuring the amount of basic compounds contained in the fluorine-containing resin particles in the outermost surface layer, the outermost surface layer is immersed in a solvent (e.g., tetrahydrofuran), and all substances other than the fluorine-containing resin particles and substances insoluble in the solvent are dissolved in the solvent (here, tetrahydrofuran), and then the solution is dropped into pure water and the precipitate is filtered. The solution containing the basic compounds obtained at this time is collected. The insoluble matter obtained by filtration is further dissolved in a solvent, and then the solution is dropped into pure water and the precipitate is filtered. This process is repeated five times, and the solutions containing the basic compounds collected in all processes are used as the measurement sample.

[0062] -measurement- Next, a solution of a basic compound with a known concentration (methanol solvent) is used, and a calibration curve (from 0 ppm to 100 ppm) is obtained from the basic compound concentration and peak area value of the solution of a basic compound with a known concentration (methanol solvent) using gas chromatography. The measurement sample is then subjected to gas chromatography, and the amount of the basic compound contained in the fluorine-containing resin particles is calculated from the obtained peak area and a calibration curve. The measurement conditions are as follows.

[0063] -Measurement conditions- Headspace sampler: (HP7694, manufactured by Hewlett-Packard Company) Measuring instrument: Gas chromatograph (HP6890 series, manufactured by HP) Detector: Flame ionization detector (FID) Column: HP19091S-433, manufactured by HP) Sample heating time: 10 min Split Ratio: 300:1 ·Flow rate: 1.0ml / min Column temperature setting: 60℃ (3min), 60℃ / min, 200℃ (1min)

[0064] ·Average particle size The average particle size of the fluorine-containing resin particles is not particularly limited, but is preferably from 0.2 μm to 4.5 μm, and more preferably from 0.2 μm to 4.0 μm. The average particle size of the fluorine-containing resin particles is a value measured by the following method. Observe with a SEM (scanning electron microscope) at a magnification of, for example, 5000 times or more, measure the maximum diameter of the fluorine-containing resin particles (secondary particles formed by aggregation of primary particles), and take the arithmetic average value obtained for 50 particles as the average particle diameter of the fluorine-containing resin particles. Note that a JEOL JSM-6700F is used as the SEM, and secondary electron images are observed at an accelerating voltage of 5 kV.

[0065] ·Specific surface area From the viewpoint of dispersion stability, the specific surface area (BET specific surface area) of the fluorine-containing resin particles is 5 m 2 / g or more 15m 2 / g or less, and 2 / g or more 13m 2 It is more preferable that the molecular weight is not more than 1 / g. The specific surface area is a value measured by a nitrogen substitution method using a BET type specific surface area measuring device (Shimadzu Corporation: Flow Soap II 2300).

[0066] ·Apparent density From the viewpoint of dispersion stability, the apparent density of the fluorine-containing resin particles is preferably from 0.2 g / ml to 0.5 g / ml, and more preferably from 0.3 g / ml to 0.45 g / ml. The apparent density is a value measured in accordance with JIS K 6891:1995.

[0067] Melting temperature The melting temperature of the fluorine-containing resin particles is preferably 300°C or higher and 340°C or lower, and more preferably 325°C or higher and 335°C or lower. The melting temperature is a melting point measured in accordance with JIS K 6891:1995.

[0068] ·Content The content of the fluorine-containing resin particles in the outermost layer is preferably from 1 mass % to 20 mass % relative to the total mass of the outermost layer, more preferably from 5 mass % to 15 mass %, and even more preferably from 7 mass % to 10 mass %.

[0069] [Fluorine-containing dispersant] The outermost layer contains a fluorine-containing dispersant. The fluorine-containing dispersant is a dispersant for the fluorine-containing resin particles, and therefore may be attached to the surfaces of the fluorine-containing resin particles. The fluorine-containing dispersant may be used alone or in combination of two or more kinds.

[0070] Examples of the fluorine-containing dispersant include a homopolymer or copolymer of a polymerizable compound having a fluorinated alkyl group (hereinafter also referred to as a "fluorinated alkyl group-containing polymer"), a fluorine-based surfactant, and the like, and it is preferable that the dispersant contains a fluorinated alkyl group-containing polymer.

[0071] Specific examples of the fluoroalkyl group-containing polymer include homopolymers of (meth)acrylates having a fluoroalkyl group, and random or block copolymers of (meth)acrylates having a fluoroalkyl group and monomers not having fluorine atoms. In this specification, (meth)acrylate means both acrylate and methacrylate.

[0072] Examples of the (meth)acrylate having a fluorinated alkyl group include 2,2,2-trifluoroethyl (meth)acrylate and 2,2,3,3,3-pentafluoropropyl (meth)acrylate.

[0073] Examples of monomers not having a fluorine atom include (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, and ethyl carbitol (meth). p)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxy (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, hydroxyethyl o-phenylphenol (meth)acrylate, o-phenylphenol glycidyl ether (meth)acrylate.

[0074] Other examples of fluorine-containing dispersants besides those mentioned above include block polymers and branched polymers disclosed in U.S. Patent No. 5,637,142 and Japanese Patent No. 4,251,662.

[0075] The fluorinated alkyl group-containing polymer preferably contains a fluorinated alkyl group-containing polymer having a structural unit represented by the following formula (FA), and more preferably contains a fluorinated alkyl group-containing polymer having a structural unit represented by the following formula (FA) and a structural unit represented by the following formula (FB).

[0076] The fluorinated alkyl group-containing polymer having a structural unit represented by the following formula (FA) and a structural unit represented by the following formula (FB) will be described below.

[0077] [ka]

[0078] In formulas (FA) and (FB), R F1 , R F2 , R F3 and R F4 each independently represents a hydrogen atom or an alkyl group. X F1 represents an alkylene chain, a halogen-substituted alkylene chain, -S-, -O-, -NH-, or a single bond. Y F1 is an alkylene chain, a halogen-substituted alkylene chain, -(C fx H 2fx-1 (OH))- or a single bond. Q F1 represents -O- or -NH-. Each of fl, fm and fn independently represents an integer of 1 or more. fp, fq, fr and fs each independently represent an integer of 0 or 1 or more. ft represents an integer between 1 and 7. fx represents an integer of 1 or greater.

[0079] In formulas (FA) and (FB), R F1 , R F2 , R F3 and R F4 The group represented by the formula (I) is preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, or the like, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.

[0080] In formulas (FA) and (FB), X F1 and Y F1 The alkylene chain (unsubstituted alkylene chain, halogen-substituted alkylene chain) represented by the formula (I) is preferably a linear or branched alkylene chain having 1 to 10 carbon atoms. Y F1 Represents -(C fx H 2fx-1 It is preferable that fx in (OH)- represents an integer of 1 or more and 10 or less. It is preferable that fp, fq, fr and fs each independently represent 0 or an integer of 1 or more and 10 or less. It is preferable that fn is, for example, 1 or more and 60 or less.

[0081] In the fluorinated alkyl group-containing polymer having a structural unit represented by formula (FA) and a structural unit represented by formula (FB), the ratio of the structural unit represented by formula (FA) to the structural unit represented by formula (FB), i.e., fl:fm, is preferably in the range of 1:9 or more and 9:1 or less, more preferably 3:7 or more and 7:3 or less.

[0082] The fluorinated alkyl group-containing polymer may be a polymer polymerized by further including a structural unit represented by formula (FC) in addition to the structural unit represented by formula (FA) and the structural unit represented by formula (FB). In this case, the content ratio of the structural unit represented by formula (FC) to the total of the structural units represented by formulas (FA) and (FB), i.e., the ratio of fl+fm (fl+fm:fz) is preferably in the range of 10:0 to 7:3, more preferably 9:1 to 7:3.

[0083] [ka]

[0084] In formula (FC), R F5 , and R F6 each independently represents a hydrogen atom or an alkyl group, and fz represents an integer of 1 or greater.

[0085] In formula (FC), R F5 , and R F6 The group represented by the formula (I) is preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, or the like, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.

[0086] Commercially available fluoroalkyl group-containing polymers include, for example, GF300, GF400 (manufactured by Toagosei Co., Ltd.), Surflon (registered trademark) series (manufactured by AGC Seimi Chemical Co., Ltd.), Ftergent series (manufactured by Neos Corporation), PF series (manufactured by Kitamura Chemical Co., Ltd.), Megafac (registered trademark) series (manufactured by DIC), and FC series (manufactured by 3M).

[0087] ·Weight average molecular weight Mw The weight average molecular weight Mw of the fluoroalkyl group-containing polymer is preferably from 20,000 to 200,000, more preferably from 50,000 to 200,000, from the viewpoint of improving the dispersibility of the fluorine-containing resin particles.

[0088] The weight average molecular weight of the fluoroalkyl group-containing polymer is a value measured by gel permeation chromatography (GPC). For example, the molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120 as a measuring device, a Tosoh TSKgel GMHHR-M + TSKgel GMHHR-M (7.8 mm I.D. 30 cm) column, and a chloroform solvent, and the molecular weight is calculated from the measurement results using a molecular weight calibration curve prepared with monodisperse polystyrene standard samples.

[0089] ·Content From the viewpoint of suppressing an increase in potential after exposure during long-term use, the content of the fluorine-containing dispersant is preferably from 0.25 mass % to 0.40 mass %, more preferably from 0.25 mass % to 0.35 mass %, and even more preferably from 0.25 mass % to 0.30 mass %, relative to the total mass of the outermost layer.

[0090] From the viewpoint of functioning as a dispersant, the content of the fluorine-containing dispersant is, for example, preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 7% by mass, relative to the fluorine-containing resin particles.

[0091] - Surface attachment method of fluorine-containing dispersant As described above, the fluorine-containing dispersant may be attached to the surface of the fluorine-containing resin particles. The method for attaching the fluorine-containing dispersant to the surface of the fluorine-containing resin particles is not particularly limited, and examples thereof include the following (1) to (3). (1) A method in which a fluorine-containing resin particle and a fluorine-containing dispersant are mixed in a dispersion solvent to prepare a dispersion liquid of the fluorine-containing resin particle. (2) A method in which fluorine-containing resin particles and a fluorine-containing dispersant are mixed using a dry powder mixer to adhere the fluorine-containing dispersant to the fluorine-containing resin particles. (3) A method in which a fluorine-containing dispersant dissolved in a solvent is dropped onto the fluorine-containing resin particles while stirring, and then the solvent is removed.

[0092] [Two or more charge transport materials] The outermost layer contains two or more charge transport materials. The two or more charge transport materials contained in the outermost layer are required to have a HOMO energy level difference between adjacent charge transport materials greater than 0 eV and not greater than 0.2 eV when the two or more charge transport materials are arranged from highest to lowest in terms of HOMO energy level.

[0093] As described above, the outermost surface layer contains two or more kinds of charge transport materials whose HOMO energy levels are not equal but are close. From the viewpoint of suppressing fluctuations in charge transport ability due to discharge products and from the viewpoint of suppressing an increase in potential after exposure during long-term use, when two or more charge transport materials are arranged from highest to lowest in terms of HOMO energy level, the difference in HOMO energy levels between adjacent charge transport materials is preferably 0.01 eV or more and 0.2 eV or less, and more preferably 0.05 eV or more and 0.15 eV or less.

[0094] From the viewpoint of charge transport ability, the charge transport material preferably has a HOMO energy level of 5.0 eV or more and 5.6 eV or less, more preferably 5.1 eV or more and 5.5 eV or less, and even more preferably 5.20 eV or more and 5.45 eV or less.

[0095] The HOMO energy level of the charge transport material is determined by the following method. That is, the ionization potential of the charge transport material measured using an air photoelectron spectrometer AC-2 manufactured by Riken Keiki Co., Ltd. is regarded as the energy level of the HOMO of the charge transport material.

[0096] Furthermore, the two or more kinds of charge transport materials contained in the outermost layer must also satisfy the following condition 1, that is, the ratio A of the content of each charge transport material to the total amount of the two or more kinds of charge transport materials. Condition 1: [(100 / N)-(100 / N×0.3)]≦A≦[(100 / N)+(100 / N×0.3)] (In condition 1, N represents the number of types of charge transport materials contained in the outermost layer.)

[0097] In other words, satisfying the above condition 1 means that, for example, when the outermost layer contains three types of charge transport materials, the content ratio A of each charge transport material satisfies (100 / 3)-(100 / N×0.3)≦A≦(100 / 3)+(100 / 3×0.3). Thus, in the outermost layer of the electrophotographic photoreceptor according to this embodiment, it is preferable that the content of each charge transport material does not vary greatly.

[0098] From the viewpoint of suppressing fluctuations in charge transport ability caused by discharge products and suppressing an increase in potential after exposure during long-term use, it is preferable that the ratio A of the content of each charge transport material to the total amount of two or more charge transport materials in the outermost layer satisfies the following condition 2, and it is more preferable that the ratio A satisfies the following condition 3. Condition 2: [(100 / N)-(100 / N×0.2)]≦A≦[(100 / N)+(100 / N×0.2)] Condition 3: [(100 / N)-(100 / N×0.1)]≦A≦[(100 / N)+(100 / N×0.1)] (In Conditions 2 and 3, N represents the number of types of charge transport materials contained in the outermost layer.)

[0099] The charge transport material contained in the outermost surface layer is not particularly limited, and examples thereof include electron transport compounds such as quinone compounds such as p-benzoquinone, chloranil, bromanil, and anthraquinone, tetracyanoquinodimethane compounds, fluorenone compounds such as 2,4,7-trinitrofluorenone, xanthone compounds, benzophenone compounds, cyanovinyl compounds, and ethylene compounds. In addition, examples of the charge transport material contained in the outermost surface layer include hole transport compounds such as triarylamine compounds, benzidine compounds, arylalkane compounds, aryl-substituted ethylene compounds, stilbene compounds, anthracene compounds, and hydrazone compounds.

[0100] Among these compounds, the preferred charge transport material from the viewpoint of charge mobility includes triarylamine compounds and benzidine compounds. Among them, the preferred triarylamine compounds are the charge transport materials represented by the following formula (CT1) (hereinafter also referred to as "butadiene-based charge transport materials"), which are an example of the triarylamine compounds. The preferred benzidine compounds are the charge transport materials represented by the following formula (CT2) (hereinafter also referred to as "benzidine-based charge transport materials").

[0101] Butadiene-based charge transport materials The butadiene-based charge transport material will be described below. The butadiene-based charge transport material is represented by the following formula (CT1).

[0102] [ka]

[0103] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 20 carbon atoms, an alkoxy group having from 1 to 20 carbon atoms, or an aryl group having from 6 to 30 carbon atoms, and two adjacent substituents may be bonded to each other to form a hydrocarbon ring structure. each independently represents 0, 1, or 2.

[0104] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, as the halogen atom, a fluorine atom and a chlorine atom are preferred, and a chlorine atom is more preferred.

[0105] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-icosyl group. Specific examples of branched alkyl groups include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, isoheptyl, sec-heptyl, tert-heptyl, isooctyl, sec-octyl, tert-octyl, isononyl, sec-nonyl, tert-nonyl, isodecyl, sec-decyl, tert-decyl, isoundecyl, sec-undecyl, tert-undecyl, neoundecyl, isododecyl, sec-dodecyl, tert-dodecyl, neododecyl, isotridecyl, sec-tridecyl, tert-tridecyl, neotridecyl, isotetradecyl, group, sec-tetradecyl group, tert-tetradecyl group, neotetradecyl group, 1-isobutyl-4-ethyloctyl group, isopentadecyl group, sec-pentadecyl group, tert-pentadecyl group, neopentadecyl group, isohexadecyl group, sec-hexadecyl group, tert-hexadecyl group, neohexadecyl group, 1-methylpentadecyl group, isoheptadecyl group, sec Examples of the isooctadecyl group include a 1-heptadecyl group, a tert-heptadecyl group, a neoheptadecyl group, an isooctadecyl group, a sec-octadecyl group, a tert-octadecyl group, a neooctadecyl group, an isononadecyl group, a sec-nonadecyl group, a tert-nonadecyl group, a neononadecyl group, a 1-methyloctyl group, an isoicosyl group, a sec-icosyl group, a tert-icosyl group, and a neoicosyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group, an ethyl group, or an isopropyl group.

[0106] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkoxy group represented by the formula (I) includes a linear or branched alkoxy group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of linear alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, an n-decyloxy group, an n-undecyloxy group, an n-dodecyloxy group, an n-tridecyloxy group, an n-tetradecyloxy group, an n-pentadecyloxy group, an n-hexadecyloxy group, an n-heptadecyloxy group, an n-octadecyloxy group, an n-nonadecyloxy group, and an n-icosyloxy group. Specific examples of branched alkoxy groups include an isopropoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, an isohexyloxy group, a sec-hexyloxy group, a tert-hexyloxy group, an isoheptyloxy group, a sec-heptyloxy group, a tert-heptyloxy group, an isooctyloxy group, a sec-octyloxy group, a tert-octyloxy group, an isononyloxy group, a se c-nonyloxy group, tert-nonyloxy group, isodecyloxy group, sec-decyloxy group, tert-decyloxy group, isoundecyloxy group, sec-undecyloxy group, tert-undecyloxy group, neoundecyloxy group, isododecyloxy group, sec-dodecyloxy group, tert-dodecyloxy group, neododecyloxy group, isotridecyloxy group, sec-tridecyloxy group, tert-tridecyloxy group, neotridecyloxy group, isotetradecyloxy group, hexadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isohept ...tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isoheptadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohex Examples of such an aryloxy group include a heptadecyloxy group, a tert-heptadecyloxy group, a neoheptadecyloxy group, an isooctadecyloxy group, a sec-octadecyloxy group, a tert-octadecyloxy group, a neooctadecyloxy group, an isononadecyloxy group, a sec-nonadecyloxy group, a tert-nonadecyloxy group, a neononadecyloxy group, a 1-methyloctyloxy group, an isoicosyloxy group, a sec-icosyloxy group, a tert-icosyloxy group, and a neoicosyloxy group. Among these, the alkoxy group is preferably a methoxy group.

[0107] In formula (CT1), R C11 , R C12, R C13 , R C14 , R C15 , and R C16 The aryl group represented by the formula (I) includes an aryl group having 6 or more and 30 or less carbon atoms (preferably 6 or more and 20 or less, more preferably 6 or more and 16 or less). Specific examples of the aryl group include a phenyl group, a naphthyl group, a phenanthryl group, and a biphenylyl group. Among these, the aryl group is preferably a phenyl group or a naphthyl group.

[0108] In addition, in formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Each of the above-mentioned substituents represented by also includes a group having a further substituent. The substituent includes the above-mentioned atoms and groups (e.g., halogen atoms, alkyl groups, alkoxy groups, aryl groups, etc.).

[0109] In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Two adjacent substituents (e.g., R C11 and R C12 Fellow, R C13 and R C14 Fellow, R C15 and R C16 In the hydrocarbon ring structure in which the substituents (atomic groups) are linked to each other, examples of the group linking the substituents to each other include a single bond, a 2,2'-methylene group, a 2,2'-ethylene group, and a 2,2'-vinylene group. Among these, a single bond and a 2,2'-methylene group are preferred. Specific examples of the hydrocarbon ring structure include a cycloalkane structure, a cycloalkene structure, and a cycloalkanepolyene structure.

[0110] In formula (CT1), n ​​and m are preferably 1.

[0111] In formula (CT1), from the viewpoint of forming a photosensitive layer (charge transport layer) with high charge transport ability, R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, and preferably, m and n each represent 1 or 2; R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 It is more preferable that m and n each represent 1. That is, the butadiene-based charge transport material (CT1) is more preferably a charge transport material represented by the following structural formula (CT1A) (exemplary compound (CT1-3)).

[0112] [ka]

[0113] Specific examples of butadiene-based charge transport materials (CT1) are shown below, but are not limited thereto. The following example compound numbers are hereinafter referred to as example compound (CT1-number). Specifically, for example, example compound 15 is hereinafter referred to as "example compound (CT1-15)".

[0114] [ka]

[0115] The abbreviations in the above exemplary compounds have the following meanings: The numbers before the substituents indicate the substitution positions on the benzene ring. -CH3: Methyl group -OCH3: Methoxy group

[0116] The butadiene-based charge transport material (CT1) may be used alone or in combination of two or more kinds.

[0117] Benzidine-based charge transport materials As the benzidine-based compound, from the viewpoint of charge mobility, a benzidine-based charge transport material (CT2) represented by the following formula (CT2) is preferably mentioned. In particular, from the viewpoint of charge mobility, it is preferable to use a butadiene-based charge transport material (CT1) and a benzidine-based charge transport material (CT2) in combination as the charge transport material.

[0118] The benzidine-based charge transport material will be described below. The benzidine-based charge transport material is represented by the following formula (CT2).

[0119] [ka]

[0120] In formula (CT2), R C21 , R C22 , and R C23 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, an alkyl group, an alkoxy group, or an aryl group.

[0121] In formula (CT2), R C21 , R C22 , and R C23 Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, as the halogen atom, a fluorine atom and a chlorine atom are preferable, and a chlorine atom is more preferable.

[0122] In formula (CT2), R C21 , R C22 , and R C23 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 10 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. Specific examples of branched alkyl groups include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, an isohexyl group, a sec-hexyl group, a tert-hexyl group, an isoheptyl group, a sec-heptyl group, a tert-heptyl group, an isooctyl group, a sec-octyl group, a tert-octyl group, an isononyl group, a sec-nonyl group, a tert-nonyl group, an isodecyl group, a sec-decyl group, and a tert-decyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group, an ethyl group, or an isopropyl group.

[0123] In formula (CT2), R C21 , R C22 , and R C23 The alkoxy group represented by the formula (I) includes a linear or branched alkoxy group having 1 to 10 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of linear alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, and an n-decyloxy group. Specific examples of branched alkoxy groups include an isopropoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, an isohexyloxy group, a sec-hexyloxy group, a tert-hexyloxy group, an isoheptyloxy group, a sec-heptyloxy group, a tert-heptyloxy group, an isooctyloxy group, a sec-octyloxy group, a tert-octyloxy group, an isononyloxy group, a sec-nonyloxy group, a tert-nonyloxy group, an isodecyloxy group, a sec-decyloxy group, and a tert-decyloxy group. Among these, the alkoxy group is preferably a methoxy group.

[0124] In formula (CT2), R C21 , R C22 , and R C23 The aryl group represented by the formula (I) includes an aryl group having 6 to 10 carbon atoms (preferably 6 to 9, more preferably 6 to 8). Specific examples of the aryl group include a phenyl group and a naphthyl group. Among these, the aryl group is preferably a phenyl group.

[0125] In addition, in formula (CT2), R C21 , R C22 , and R C23 Each of the above-mentioned substituents represented by also includes a group having a further substituent. The substituent includes the above-mentioned atoms and groups (e.g., halogen atoms, alkyl groups, alkoxy groups, aryl groups, etc.).

[0126] In formula (CT2), from the viewpoint of forming a photosensitive layer (charge transport layer) having a high charge transport ability, R C21 , R C22 , and R C23 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R C21 , R C22 , and R C23 represents a hydrogen atom, and R C22 More preferably, represents an alkyl group having 1 to 10 carbon atoms (particularly, a methyl group). Specifically, the benzidine-based charge transport material (CT2) is particularly preferably a charge transport material represented by the following structural formula (CT2A) (exemplary compound (CT2-2)).

[0127] [ka]

[0128] Specific examples of the charge transport material represented by formula (CT2) are shown below, but are not limited thereto. The following exemplary compound numbers are hereinafter referred to as exemplary compound (CT2-number). Specifically, for example, exemplary compound 15 is hereinafter referred to as "exemplary compound (CT2-15)".

[0129] [ka]

[0130] The abbreviations in the above exemplary compounds have the following meanings: The numbers before the substituents indicate the substitution positions on the benzene ring. -CH3: Methyl group -C2H5: Ethyl group -OCH3: Methoxy group -OC2H5: Ethoxy group

[0131] The benzidine-based charge transport material (CT2) may be used alone or in combination of two or more kinds.

[0132] As the charge transport material, a polymer charge transport material may be used. As the polymer charge transport material, known materials having charge transport properties such as poly-N-vinylcarbazole, polysilane, etc. are used. In particular, polyester polymer charge transport materials disclosed in JP-A-8-176293, JP-A-8-208820, etc. are particularly preferred.

[0133] The total content of the charge transport material may be determined depending on the type of the outermost layer. For example, the total content of the charge transport material is preferably 30% by mass or more and 60% by mass or less, more preferably 35% by mass or more and 55% by mass or less, and even more preferably 30% by mass or more and 50% by mass or less, based on the total amount of the outermost layer. The above-mentioned range of the content of the charge transport material is suitable, for example, when the outermost layer is a charge transport layer.

[0134] [Surface roughness Ra] The surface roughness Ra of the outermost layer (i.e., the surface roughness Ra of the electrophotographic photoreceptor according to this embodiment) is preferably 0.13 μm or less, more preferably 0.10 μm or less, and even more preferably 0.08 μm or less, from the viewpoint of enhancing the surface smoothness of the photoreceptor. On the other hand, the lower limit of the surface roughness Ra of the outermost layer is preferably, for example, 0.05 μm or more.

[0135] The surface roughness Ra is determined by the following method. A part of the outermost surface layer is cut out with a cutter or the like to obtain a test piece. The test piece is measured using a stylus type surface roughness measuring instrument (Surfcom 1400A: manufactured by Tokyo Seimitsu Co., Ltd., etc.). The measurement conditions are in accordance with JIS B 0601:1994, with evaluation length Ln = 10 mm, reference length L = 0.8 mm, and cutoff value = 0.8 mm.

[0136] <Conductive substrate> Examples of the conductive substrate include metal plates, metal drums, and metal belts containing metals (aluminum, copper, zinc, chromium, nickel, molybdenum, vanadium, indium, gold, platinum, etc.) or alloys (stainless steel, etc.). Examples of the conductive substrate include paper, resin films, belts, etc. coated, vapor-deposited, or laminated with a conductive compound (e.g., conductive polymer, indium oxide, etc.), a metal (e.g., aluminum, palladium, gold, etc.), or an alloy. Here, "conductive" means that the volume resistivity is 10 13 This means that the resistance is less than Ωcm.

[0137] When the electrophotographic photoreceptor is used in a laser printer, the surface of the conductive substrate is preferably roughened to a center line average roughness Ra of 0.04 μm to 0.5 μm in order to suppress interference fringes that occur when irradiating with laser light. When non-interfering light is used as the light source, roughening to prevent interference fringes is not particularly necessary, but it is suitable for extending the life of the conductive substrate since it suppresses the occurrence of defects due to unevenness on the surface.

[0138] Examples of methods for roughening the surface include wet honing, which involves spraying an abrasive suspended in water onto the conductive substrate; centerless grinding, in which the conductive substrate is pressed against a rotating grindstone and continuously ground; and anodizing.

[0139] As a method for roughening the surface, there can be mentioned a method in which, without roughening the surface of the conductive substrate, a conductive or semiconductive powder is dispersed in a resin to form a layer on the surface of the conductive substrate, and the surface is roughened by the particles dispersed in the layer.

[0140] In the roughening treatment by anodization, an oxide film is formed on the surface of a conductive substrate made of metal (e.g., aluminum) by anodizing the substrate in an electrolyte solution using the substrate as the anode. Examples of electrolyte solutions include sulfuric acid solution and oxalic acid solution. However, the porous anodic oxide film formed by anodization is chemically active in its original state, easily contaminated, and has a large resistance variation depending on the environment. Therefore, it is preferable to perform a sealing treatment on the porous anodic oxide film, in which the micropores of the oxide film are filled by volume expansion caused by hydration reaction in pressurized steam or boiling water (metal salts such as nickel may be added) to change the film into a more stable hydrated oxide.

[0141] The thickness of the anodic oxide film is preferably, for example, from 0.3 μm to 15 μm. If the thickness is within this range, the film tends to exhibit a barrier property against injection and tends to suppress an increase in residual potential due to repeated use.

[0142] The conductive substrate may be subjected to a treatment with an acidic treatment solution or a boehmite treatment. Treatment with an acid treatment liquid is carried out, for example, as follows. First, an acid treatment liquid containing phosphoric acid, chromic acid, and hydrofluoric acid is prepared. The compounding ratios of phosphoric acid, chromic acid, and hydrofluoric acid in the acid treatment liquid are, for example, in the range of 10% by mass to 11% by mass for phosphoric acid, 3% by mass to 5% by mass for chromic acid, and 0.5% by mass to 2% by mass for hydrofluoric acid, and the total concentration of these acids is preferably in the range of 13.5% by mass to 18% by mass. The treatment temperature is preferably, for example, 42° C. to 48° C. The film thickness of the coating is preferably 0.3 μm to 15 μm.

[0143] The boehmite treatment is carried out, for example, by immersing the plate in pure water at 90° C. to 100° C. for 5 to 60 minutes, or by contacting the plate with heated steam at 90° C. to 120° C. for 5 to 60 minutes. The thickness of the coating is preferably 0.1 μm to 5 μm. This may be further anodized using an electrolyte solution having low coating solubility, such as adipic acid, boric acid, borates, phosphates, phthalates, maleates, benzoates, tartrates, or citrates.

[0144] ≪Sublayer≫ The undercoat layer is, for example, a layer containing inorganic particles and a binder resin.

[0145] As inorganic particles, for example, powder resistivity (volume resistivity) of 10 2 Ωcm or more 10 11 Examples of such particles include inorganic particles with a particle size of Ωcm or less. Among these, examples of inorganic particles having the above-mentioned resistance value include metal oxide particles such as tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles, and zinc oxide particles are particularly preferred.

[0146] The specific surface area of ​​inorganic particles by the BET method is, for example, 10 m 2 / g or higher is preferable. The volume average particle size of the inorganic particles is, for example, from 50 nm to 2000 nm (preferably from 60 nm to 1000 nm).

[0147] The content of the inorganic particles is, for example, preferably from 10% by mass to 80% by mass, more preferably from 40% by mass to 80% by mass, based on the binder resin.

[0148] The inorganic particles may be surface-treated. Two or more types of inorganic particles having different surface treatments or different particle sizes may be used in combination.

[0149] Examples of the surface treatment agent include a silane coupling agent, a titanate coupling agent, an aluminum coupling agent, a surfactant, etc. In particular, a silane coupling agent is preferred, and a silane coupling agent having an amino group is more preferred.

[0150] Examples of silane coupling agents having an amino group include, but are not limited to, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane.

[0151] Silane coupling agents may be used in combination of two or more kinds. For example, a silane coupling agent having an amino group may be used in combination with another silane coupling agent. Examples of other silane coupling agents include, but are not limited to, vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.

[0152] The surface treatment method using the surface treatment agent may be any known method, and may be either a dry method or a wet method.

[0153] The amount of the surface treatment agent to be used is preferably, for example, 0.5% by mass or more and 10% by mass or less based on the inorganic particles.

[0154] Here, it is preferable that the undercoat layer contains an electron accepting compound (acceptor compound) together with the inorganic particles, from the viewpoints of improving the long-term stability of electrical properties and carrier blocking properties.

[0155] Examples of the electron-accepting compound include electron-transporting substances such as quinone compounds such as chloranil and bromoanil; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone and 2,4,5,7-tetranitro-9-fluorenone; oxadiazole compounds such as 2-(4-biphenyl)-5-(4-t-butylphenyl)-1,3,4-oxadiazole, 2,5-bis(4-naphthyl)-1,3,4-oxadiazole and 2,5-bis(4-diethylaminophenyl)-1,3,4-oxadiazole; xanthone compounds; thiophene compounds; and diphenoquinone compounds such as 3,3',5,5'-tetra-t-butyldiphenoquinone. In particular, the electron-accepting compound is preferably a compound having an anthraquinone structure. Examples of the compound having an anthraquinone structure include hydroxyanthraquinone compounds, aminoanthraquinone compounds, and aminohydroxyanthraquinone compounds, and more specifically, anthraquinone, alizarin, quinizarin, anthrarufin, and purpurin.

[0156] The electron accepting compound may be contained in the undercoat layer in a dispersed state together with the inorganic particles, or may be contained in a state of being attached to the surfaces of the inorganic particles.

[0157] The method for attaching the electron accepting compound to the surface of the inorganic particles may be, for example, a dry method or a wet method.

[0158] The dry method is, for example, a method in which an electron-accepting compound is attached to the surface of inorganic particles by dropping an electron-accepting compound directly or dissolved in an organic solvent or spraying it together with dry air or nitrogen gas while stirring inorganic particles with a mixer or the like that exerts a large shearing force. The dropping or spraying of the electron-accepting compound is preferably performed at a temperature below the boiling point of the solvent. After dropping or spraying the electron-accepting compound, baking may be performed at 100° C. or higher. The temperature and time of baking are not particularly limited as long as electrophotographic properties can be obtained.

[0159] The wet method is a method in which, for example, an electron-accepting compound is added while dispersing inorganic particles in a solvent by stirring, ultrasonic waves, a sand mill, an attritor, a ball mill, etc., and the inorganic particles are stirred or dispersed, and then the solvent is removed to attach the electron-accepting compound to the surface of the inorganic particles. The solvent is removed, for example, by filtration or distillation. After the solvent is removed, baking may be performed at 100°C or higher. The baking temperature and time are not particularly limited as long as electrophotographic properties are obtained. In the wet method, moisture contained in the inorganic particles may be removed before adding the electron-accepting compound, and examples of such methods include a method of removing the moisture while stirring and heating in a solvent, and a method of removing the moisture by azeotropy with the solvent.

[0160] The attachment of the electron accepting compound may be carried out before or after the inorganic particles are subjected to a surface treatment with a surface treatment agent, or the attachment of the electron accepting compound and the surface treatment with the surface treatment agent may be carried out simultaneously.

[0161] The content of the electron accepting compound is, for example, from 0.01% by mass to 20% by mass, and preferably from 0.01% by mass to 10% by mass, based on the inorganic particles.

[0162] Examples of the binder resin used in the undercoat layer include known materials such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, unsaturated polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, alkyd resins, and epoxy resins; zirconium chelate compounds; titanium chelate compounds; aluminum chelate compounds; titanium alkoxide compounds; organic titanium compounds; and silane coupling agents. Examples of the binder resin used in the undercoat layer include charge transporting resins having charge transporting groups, conductive resins (such as polyaniline, etc.), and the like.

[0163] Among these, the binder resin used in the undercoat layer is preferably a resin that is insoluble in the coating solvent of the upper layer, and in particular, a resin obtained by reacting at least one resin selected from the group consisting of thermosetting resins such as urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, unsaturated polyester resins, alkyd resins, and epoxy resins, with a curing agent is preferred. When two or more of these binder resins are used in combination, the mixing ratio is set as necessary.

[0164] The undercoat layer may contain various additives for improving electrical properties, environmental stability, and image quality. Examples of the additives include known materials such as polycyclic condensation and azo-based electron transport pigments, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, silane coupling agents, etc. As described above, silane coupling agents are used for surface treatment of inorganic particles, and may also be added to the undercoat layer as an additive.

[0165] Examples of silane coupling agents as additives include vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, and the like.

[0166] Examples of the zirconium chelate compound include zirconium butoxide, zirconium ethyl acetoacetate, zirconium triethanolamine, acetylacetonate zirconium butoxide, ethyl acetoacetate zirconium butoxide, zirconium acetate, zirconium oxalate, zirconium lactate, zirconium phosphonate, zirconium octanoate, zirconium naphthenate, zirconium laurate, zirconium stearate, zirconium isostearate, methacrylate zirconium butoxide, stearate zirconium butoxide, and isostearate zirconium butoxide.

[0167] Examples of titanium chelate compounds include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, polytitanium acetylacetonate, titanium octylene glycolate, titanium lactate ammonium salt, titanium lactate, titanium lactate ethyl ester, titanium triethanolamine, and polyhydroxytitanium stearate.

[0168] Examples of aluminum chelate compounds include aluminum isopropylate, monobutoxyaluminum diisopropylate, aluminum butyrate, diethylacetoacetate aluminum diisopropylate, and aluminum tris(ethylacetoacetate).

[0169] These additives may be used alone or as a mixture or polycondensation product of a plurality of compounds.

[0170] The undercoat layer preferably has a Vickers hardness of 35 or more. The surface roughness (ten-point average roughness) of the undercoat layer is preferably adjusted to between 1 / (4n) (n is the refractive index of the upper layer) and 1 / 2 of the wavelength λ of the exposure laser used in order to suppress moire images. Resin particles or the like may be added to the undercoat layer to adjust the surface roughness. Examples of the resin particles include silicone resin particles and crosslinked polymethyl methacrylate resin particles. The surface of the undercoat layer may be polished to adjust the surface roughness. Examples of the polishing method include buffing, sandblasting, wet honing, grinding, and the like.

[0171] The formation of the undercoat layer is not particularly limited, and a well-known formation method can be used. For example, the undercoat layer can be formed by forming a coating film of a coating solution for forming the undercoat layer in which the above-mentioned components are added to a solvent, drying the coating film, and heating it as necessary.

[0172] Examples of the solvent for preparing the coating liquid for forming the undercoat layer include known organic solvents, such as alcohol-based solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, ketone-based solvents, ketone alcohol-based solvents, ether-based solvents, and ester-based solvents. Specific examples of these solvents include ordinary organic solvents such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, ethyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, and toluene.

[0173] Examples of the method for dispersing the inorganic particles when preparing the coating liquid for forming the undercoat layer include known methods such as those using a roll mill, a ball mill, a vibrating ball mill, an attritor, a sand mill, a colloid mill, and a paint shaker.

[0174] Examples of the method for applying the coating liquid for forming the undercoat layer onto the conductive substrate include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.

[0175] The thickness of the undercoat layer is set, for example, preferably at least 15 μm, and more preferably within the range of from 20 μm to 50 μm.

[0176] <Middle Class> Although not shown, an intermediate layer may be further provided between the undercoat layer and the photosensitive layer. The intermediate layer is, for example, a layer containing a resin. Examples of the resin used in the intermediate layer include polymer compounds such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, phenol-formaldehyde resins, and melamine resins. The intermediate layer may be a layer containing an organometallic compound. Examples of the organometallic compound used in the intermediate layer include organometallic compounds containing metal atoms such as zirconium, titanium, aluminum, manganese, and silicon. The compounds used in the intermediate layer may be used alone or as a mixture or polycondensation product of a plurality of compounds.

[0177] Among these, the intermediate layer is preferably a layer containing an organometallic compound containing zirconium atoms or silicon atoms.

[0178] The formation of the intermediate layer is not particularly limited, and a well-known formation method can be used. For example, the intermediate layer can be formed by forming a coating film of a coating liquid for forming an intermediate layer in which the above components are added to a solvent, drying the coating film, and heating it if necessary. The intermediate layer can be formed by any of the usual coating methods, such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating and curtain coating.

[0179] The thickness of the intermediate layer is preferably set in the range of, for example, 0.1 μm to 3 μm. The intermediate layer may also be used as an undercoat layer.

[0180] <Charge generation layer> The charge generation layer is, for example, a layer containing a charge generation material and a binder resin. The charge generation layer may also be a vapor deposition layer of the charge generation material. The vapor deposition layer of the charge generation material is suitable for use with a non-coherent light source such as an LED (Light Emitting Diode) or an organic EL (Electro-Luminescence) image array.

[0181] Examples of the charge generating material include azo pigments such as bisazo and trisazo; condensed aromatic pigments such as dibromoanthanthrone; perylene pigments; pyrrolopyrrole pigments; phthalocyanine pigments; zinc oxide; and trigonal selenium.

[0182] Among these, in order to correspond to the laser exposure in the near infrared region, it is preferable to use a metal phthalocyanine pigment or a metal-free phthalocyanine pigment as the charge generating material.Specifically, for example, hydroxygallium phthalocyanine disclosed in JP-A-5-263007, JP-A-5-279591, etc., chlorogallium phthalocyanine disclosed in JP-A-5-98181, etc., dichlorotin phthalocyanine disclosed in JP-A-5-140472, JP-A-5-140473, etc., and titanyl phthalocyanine disclosed in JP-A-4-189873, etc. are more preferable.

[0183] On the other hand, in order to accommodate laser exposure in the near ultraviolet region, preferred charge generating materials include condensed aromatic pigments such as dibromoanthanthrone, thioindigo pigments, porphyrazine compounds, zinc oxide, trigonal selenium, and the bisazo pigments disclosed in JP-A-2004-78147 and JP-A-2005-181992.

[0184] The above charge generating materials may be used when using incoherent light sources such as LEDs and organic EL image arrays that emit light at a central wavelength of 450 nm to 780 nm, but from the viewpoint of resolution, when using a thin photosensitive layer of 20 μm or less, the electric field strength in the photosensitive layer becomes high, and a decrease in charging due to charge injection from the substrate, so-called black spots, is likely to occur as an image defect. This becomes more noticeable when using charge generating materials that are p-type semiconductors such as trigonal selenium and phthalocyanine pigments and are prone to generating dark current.

[0185] In contrast, when an n-type semiconductor such as a fused aromatic pigment, a perylene pigment, or an azo pigment is used as the charge generating material, dark current is unlikely to occur, and image defects called black spots can be suppressed even when the material is a thin film. Examples of n-type charge generating materials include, but are not limited to, compounds (CG-1) to (CG-27) described in paragraphs

[0288] to

[0291] of JP-A-2012-155282. The n-type is determined by the polarity of the photocurrent that flows using the commonly used time-of-flight method, and those that easily pass electrons as carriers rather than holes are considered to be n-type.

[0186] The binder resin used in the charge generating layer may be selected from a wide range of insulating resins, and may also be selected from organic photoconductive polymers such as poly-N-vinylcarbazole, polyvinylanthracene, polyvinylpyrene, polysilane, and the like. Examples of the binder resin include polyvinyl butyral resin, polyarylate resin (polycondensation product of bisphenols and aromatic dicarboxylic acid, etc.), polycarbonate resin, polyester resin, phenoxy resin, vinyl chloride-vinyl acetate copolymer, polyamide resin, acrylic resin, polyacrylamide resin, polyvinylpyridine resin, cellulose resin, urethane resin, epoxy resin, casein, polyvinyl alcohol resin, polyvinylpyrrolidone resin, etc. Here, "insulating" means a material having a volume resistivity of 10 13 This means that the resistance is Ωcm or more. These binder resins may be used alone or in combination of two or more.

[0187] The compounding ratio of the charge generating material to the binder resin is preferably within a range of 10:1 to 1:10 by mass.

[0188] The charge generating layer may contain other well-known additives.

[0189] The formation of the charge generation layer is not particularly limited, and a known formation method is used, for example, by forming a coating film of a coating solution for forming a charge generation layer in which the above-mentioned components are added to a solvent, drying the coating film, and heating it as necessary. The formation of the charge generation layer may be performed by vapor deposition of a charge generation material. The formation of the charge generation layer by vapor deposition is particularly suitable when a condensed ring aromatic pigment or a perylene pigment is used as the charge generation material.

[0190] Examples of the solvent for preparing the coating liquid for forming the charge generating layer include methanol, ethanol, n-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, toluene, etc. These solvents may be used alone or in combination of two or more.

[0191] Examples of methods for dispersing particles (e.g., charge generating material) in the coating liquid for forming a charge generating layer include media dispersers such as ball mills, vibration ball mills, attritors, sand mills, and horizontal sand mills, and medialess dispersers such as stirrers, ultrasonic dispersers, roll mills, and high-pressure homogenizers. Examples of high-pressure homogenizers include a collision method in which the dispersion liquid is dispersed by liquid-liquid collision or liquid-wall collision under high pressure, and a penetration method in which the dispersion liquid is dispersed by penetrating a fine flow path under high pressure. During this dispersion, it is effective to adjust the average particle size of the charge generating material in the coating liquid for forming the charge generating layer to 0.5 μm or less, preferably 0.3 μm or less, and more preferably 0.15 μm or less.

[0192] Examples of a method for applying the coating liquid for forming the charge generating layer onto the undercoat layer (or onto the intermediate layer) include conventional methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.

[0193] The drying temperature for the coating film obtained by coating the coating liquid for forming the charge generating layer on the undercoat layer (or on the intermediate layer) is preferably, for example, 30° C. or more and 80° C. or less.

[0194] The thickness of the charge generating layer is set, for example, preferably in the range of 0.1 μm or more and 5.0 μm or less, and more preferably in the range of 0.2 μm or more and 2.0 μm or less.

[0195] ≪Charge transport layer≫ The charge transport layer is, for example, a layer containing a charge transport material and a binder resin. When the charge transport layer is the outermost layer, it is preferable that the charge transport layer contains fluorine-containing resin particles, a fluorine-containing dispersant, two or more kinds of charge transport materials, and a binder resin. The charge transport layer, which is the outermost layer, has the above-mentioned relationship between the HOMO energy levels of the two or more kinds of charge transport materials, and the content ratio A of each charge transport material also satisfies the above-mentioned condition 1.

[0196] The charge transport material contained in the charge transport layer is the same as the charge transport material contained in the outermost layer, and the preferred embodiments are also the same.

[0197] Examples of the binder resin used in the charge transport layer include polycarbonate resin, polyester resin, polyarylate resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, styrene-butadiene copolymer, vinylidene chloride-acrylonitrile copolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-maleic anhydride copolymer, silicone resin, silicone alkyd resin, phenol-formaldehyde resin, styrene-alkyd resin, poly-N-vinylcarbazole, polysilane, etc. Among these, polycarbonate resin or polyarylate resin is preferable as the binder resin. The binder resin may be used alone or in combination of two or more kinds.

[0198] The compounding ratio of the charge transport material to the binder resin is preferably 10:1 or more and 1:5 or less in mass ratio.

[0199] When fluorine-containing resin particles having many carboxy groups are used together with a polycarbonate resin, the dispersibility of the fluorine-containing resin particles tends to decrease. In particular, when a polycarbonate resin (also called a specific polycarbonate resin) containing a structural unit represented by the following formula (PCA) and a structural unit represented by the following formula (PCB), which has many carbonate groups (-OC(=O)O-) per unit mole, is used, the dispersibility of the fluorine-containing resin particles tends to decrease. Therefore, when a polycarbonate resin containing a structural unit represented by the following formula (PCA) and a structural unit represented by the following formula (PCB) is used, the dispersibility of the fluorine-containing resin particles tends to decrease when the number of carboxy groups is more than 10 carbon atoms. 6 It is preferable to use 0 to 30 fluorine-containing resin particles per piece.

[0200] [ka]

[0201] In the formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and RP4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 5 to 7 carbon atoms, or an aryl group having 6 to 12 carbon atoms. P1 represents a phenylene group, a biphenylylene group, a naphthylene group, an alkylene group, or a cycloalkylene group.

[0202] In the formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 6 carbon atoms (preferably 1 to 3 carbon atoms). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, and an n-hexyl group. Specific examples of branched alkyl groups include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, an isohexyl group, a sec-hexyl group, and a tert-hexyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group or an ethyl group.

[0203] In the formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 Examples of the cycloalkyl group represented by the formula (I) include a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group.

[0204] In the formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 Examples of the aryl group represented by the formula (I) include a phenyl group, a naphthyl group, and a biphenylyl group.

[0205] In the formulas (PCA) and (PCB), X P1The alkylene group represented by the formula (I) includes a linear or branched alkylene group having 1 to 12 carbon atoms (preferably 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms). Specific examples of the linear alkylene group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, an n-decylene group, an n-undecylene group, and an n-dodecylene group. Specific examples of branched alkylene groups include isopropylene, isobutylene, sec-butylene, tert-butylene, isopentylene, neopentylene, tert-pentylene, isohexylene, sec-hexylene, tert-hexylene, isoheptylene, sec-heptylene, tert-heptylene, isooctylene, sec-octylene, tert-octylene, isononylene, sec-nonylene, tert-nonylene, isodecylene, sec-decylene, tert-decylene, isoundecylene, sec-undecylene, tert-undecylene, neoundecylene, isododecylene, sec-dodecylene, tert-dodecylene, and neododecylene. Among these, the alkylene group is preferably a lower alkyl group such as a methylene group, an ethylene group, or a butylene group.

[0206] In the formulas (PCA) and (PCB), X P1 The cycloalkylene group represented by the formula (I) includes a cycloalkylene group having 3 to 12 carbon atoms (preferably a cycloalkylene group having 3 to 10 carbon atoms, more preferably a cycloalkylene group having 5 to 8 carbon atoms). Specific examples of the cycloalkylene group include a cyclopropylene group, a cyclopentylene group, a cyclohexylene group, a cyclooctylene group, and a cyclododecanylene group. Among these, the cycloalkylene group is preferably a cyclohexylene group.

[0207] In the formulas (PCA) and (PCB), R P1 , RP2 , R P3 , R P4 , and X P1 Each of the above-mentioned substituents represented by also includes groups having a further substituent. Examples of the substituent include a halogen atom (e.g., a fluorine atom, a chlorine atom), an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a cycloalkyl group (e.g., a cycloalkyl group having 5 to 7 carbon atoms), an alkoxy group (e.g., an alkoxy group having 1 to 4 carbon atoms), and an aryl group (e.g., a phenyl group, a naphthyl group, a biphenylyl group, etc.).

[0208] In the formula (PCA), R P1 , and R P2 each independently preferably represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R P1 , and R P2 More preferably, represents a hydrogen atom. In the formula (PCB), R P3 , and R P4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; X P1 It is preferred that represents an alkylene group or a cycloalkylene group.

[0209] Specific examples of the specific polycarbonate resin include, but are not limited to, the following: In the example compounds, pm and pn indicate copolymerization ratios.

[0210] [ka]

[0211] Here, in the specific polycarbonate resin, the content (copolymerization ratio) of the structural unit represented by formula (PCA) is in the range of 5 mol % or more and 95 mol % or less, preferably 5 mol % or more and 50 mol % or less, and more preferably 15 mol % or more and 30 mol % or less, based on all structural units constituting the polycarbonate resin. Specifically, in the above example compounds of the specific polycarbonate resin, pm and pn indicate the copolymerization ratio (molar ratio), and pm:pn is in the range of 95:5 to 5:95, 50:50 to 5:95, and more preferably 15:85 to 30:70.

[0212] The compounding ratio of the charge transport material to the binder resin is preferably from 10:1 to 1:5 by mass.

[0213] The charge transport layer may contain other well-known additives.

[0214] The formation of the charge transport layer is not particularly limited, and a known formation method can be used. For example, the charge transport layer can be formed by forming a coating film of a coating liquid for forming the charge transport layer in which the above components are added to a solvent, drying the coating film, and heating it as necessary.

[0215] Examples of solvents for preparing the coating liquid for forming the charge transport layer include ordinary organic solvents such as aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene, ketones such as acetone and 2-butanone, halogenated aliphatic hydrocarbons such as methylene chloride, chloroform, and ethylene chloride, and cyclic or linear ethers such as tetrahydrofuran and ethyl ether. These solvents may be used alone or in combination of two or more.

[0216] Examples of a coating method for coating the coating liquid for forming the charge transport layer on the charge generating layer include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating and curtain coating.

[0217] The thickness of the charge transport layer is set, for example, preferably in the range of 5 μm or more and 50 μm or less, and more preferably in the range of 10 μm or more and 30 μm or less.

[0218] ≪Surface protective layer≫ If necessary, a surface protective layer is provided on the photosensitive layer. The surface protective layer is provided for the purpose of, for example, preventing chemical changes in the photosensitive layer when it is charged, and further improving the mechanical strength of the photosensitive layer. For this reason, the surface protective layer may be a layer made of a cured film (crosslinked film). In the electrophotographic photoreceptor having a surface protective layer, the surface protective layer is the outermost layer. Therefore, in the electrophotographic photoreceptor having a surface protective layer, the surface protective layer contains fluorine-containing resin particles, a fluorine-containing dispersant, and two or more kinds of charge transport materials, the relationship between the HOMO energy levels of the two or more kinds of charge transport materials is as described above, and the content ratio A of each charge transport material also satisfies the above-mentioned condition 1.

[0219] Examples of the surface protective layer made of a cured film include the following layers 1) and 2). (1) A layer composed of a cured film of a composition containing a reactive group-containing charge transport material having a reactive group and a charge transport skeleton in the same molecule (i.e., a layer containing a polymer or crosslinked body of the reactive group-containing charge transport material). (2) A layer composed of a cured film of a composition containing a non-reactive charge transport material and a reactive group-containing non-charge transport material that does not have a charge transport skeleton and has a reactive group (i.e., a layer containing a non-reactive charge transport material and a polymer or crosslinked product of the reactive group-containing non-charge transport material).

[0220] The reactive group of the reactive group-containing charge transport material may be a chain polymerizable group, an epoxy group, -OH, -OR (wherein R represents an alkyl group), -NH2, -SH, -COOH, or -SiR. Q1 3-Qn (OR Q2 ) Qn [However, R Q1 represents a hydrogen atom, an alkyl group, or a substituted or unsubstituted aryl group; R Q2 represents a hydrogen atom, an alkyl group, or a trialkylsilyl group; Qn represents an integer of 1 to 3.

[0221] The chain polymerizable group is not particularly limited as long as it is a functional group capable of radical polymerization, and is, for example, a functional group having a group containing at least a carbon double bond.Specific examples include a group containing at least one selected from a vinyl group, a vinyl ether group, a vinyl thioether group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof.Among them, the chain polymerizable group is preferably a group containing at least one selected from a vinyl group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof, because of its excellent reactivity.

[0222] The charge transporting skeleton of the reactive group-containing charge transporting material is not particularly limited as long as it is a known structure in electrophotographic photoreceptors, and examples thereof include a skeleton derived from a nitrogen-containing hole transporting compound such as a triarylamine compound, a benzidine compound, a hydrazone compound, etc., and a structure conjugated with a nitrogen atom. Among these, a triarylamine skeleton is preferred.

[0223] The reactive group-containing charge transport material having a reactive group and a charge transporting skeleton, the non-reactive charge transport material, and the reactive group-containing non-charge transport material may be selected from well-known materials.

[0224] The surface protective layer may contain other well-known additives.

[0225] The formation of the surface protection layer is not particularly limited, and a well-known formation method can be used. For example, the surface protection layer can be formed by forming a coating film of a coating liquid for forming the surface protection layer in which the above components are added to a solvent, drying the coating film, and, if necessary, subjecting it to a curing treatment such as heating.

[0226] Examples of solvents for preparing a coating liquid for forming a surface protective layer include aromatic solvents such as toluene and xylene, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ester solvents such as ethyl acetate and butyl acetate, ether solvents such as tetrahydrofuran and dioxane, cellosolve solvents such as ethylene glycol monomethyl ether, and alcohol solvents such as isopropyl alcohol and butanol. These solvents may be used alone or in combination of two or more. The coating liquid for forming the surface protective layer may be a solvent-free coating liquid.

[0227] Examples of a method for applying the coating liquid for forming a surface protective layer onto a photosensitive layer (e.g., a charge transport layer) include conventional methods such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating, and curtain coating.

[0228] The thickness of the surface protective layer is set, for example, preferably in the range of 1 μm or more and 20 μm or less, and more preferably in the range of 2 μm or more and 10 μm or less.

[0229] <Single-layer photosensitive layer> The single-layer type photosensitive layer (charge generating / charge transporting layer) is, for example, a layer containing a charge generating material, a charge transporting material, and, if necessary, a binder resin and other well-known additives. When the single-layer photosensitive layer is the outermost layer, the single-layer photosensitive layer preferably contains fluorine-containing resin particles, a fluorine-containing dispersant, two or more kinds of charge transport materials, a charge generating material, and a binder resin. The single-layer photosensitive layer that is the outermost layer has the above-mentioned relationship between the HOMO energy levels of the two or more kinds of charge transport materials, and the content ratio A of each charge transport material also satisfies the above-mentioned condition 1.

[0230] The materials contained in the single-layer photosensitive layer are the same as those described in the charge generating layer and the charge transport layer. The content of the charge generating material in the single-layer photosensitive layer is preferably 0.1% by mass to 10% by mass, more preferably 0.8% by mass to 5% by mass, based on the total solid content. The content of the charge transport material in the single-layer photosensitive layer is preferably 5% by mass to 50% by mass, based on the total solid content. The method for forming the single-layer type photosensitive layer is the same as the method for forming the charge generating layer and the charge transport layer. The thickness of the single-layer photosensitive layer is, for example, 5 μm or more and 50 μm or less, and preferably 10 μm or more and 40 μm or less.

[0231] <Activation Energy> In the electrophotographic photoreceptor according to the present embodiment, from the viewpoint of suppressing fluctuations in charge transport ability caused by discharge products and from the viewpoint of being able to suppress an increase in potential after exposure during long-term use, the activation energy is preferably 0.35 eV or less, and more preferably 0.2 eV or more and 0.35 eV or less.

[0232] Here, the activation energy of the electrophotographic photosensitive member is a value measured by the following method. That is, the activation energy of the electrophotographic photoreceptor is measured by using a thermally stimulated current (TSC) measurement. Specifically, an electron trap measurement system (TS-FETT) from Rigaku Corporation is used to create a trap accumulation state by irradiating ultraviolet light at -150°C, and then the activation energy is calculated by measuring the current that flows when the temperature is raised from -150°C to 50°C at a rate of 10°C / min.

[0233] -Image forming apparatus and process cartridge- The image forming apparatus according to the present embodiment includes an electrophotographic photoreceptor, a charging unit for charging the surface of the electrophotographic photoreceptor, an electrostatic latent image forming unit for forming an electrostatic latent image on the surface of the charged electrophotographic photoreceptor, a developing unit for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing toner to form a toner image, and a transfer unit for transferring the toner image to the surface of a recording medium. The electrophotographic photoreceptor according to the present embodiment described above is applied as the electrophotographic photoreceptor.

[0234] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as an apparatus provided with a fixing means for fixing a toner image transferred onto the surface of a recording medium; an apparatus of a direct transfer type for directly transferring a toner image formed on the surface of an electrophotographic photosensitive member onto a recording medium; an apparatus of an intermediate transfer type for primarily transferring a toner image formed on the surface of an electrophotographic photosensitive member onto the surface of an intermediate transfer member, and then secondarily transferring the toner image transferred onto the surface of the intermediate transfer member onto the surface of a recording medium; an apparatus provided with a cleaning means for cleaning the surface of an electrophotographic photosensitive member before charging after the transfer of a toner image; an apparatus provided with a discharging means for irradiating the surface of an electrophotographic photosensitive member with discharging light to discharge the surface before charging after the transfer of a toner image; and an apparatus provided with an electrophotographic photosensitive member heating member for increasing the temperature of the electrophotographic photosensitive member and reducing the relative temperature.

[0235] In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the electrophotographic photosensitive body onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0236] The image forming apparatus according to the present embodiment may be either a dry development type image forming apparatus or a wet development type image forming apparatus (a development type using a liquid developer).

[0237] In the image forming apparatus according to the present embodiment, for example, a portion including an electrophotographic photoreceptor may be a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including the electrophotographic photoreceptor according to the present embodiment is preferably used. In addition to the electrophotographic photoreceptor, the process cartridge may include at least one selected from the group consisting of a charging means, an electrostatic latent image forming means, a developing means, and a transfer means.

[0238] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.

[0239] FIG. 2 is a schematic diagram showing an example of the image forming apparatus according to the present embodiment. As shown in FIG. 2, the image forming apparatus 100 according to the present embodiment includes a process cartridge 300 including an electrophotographic photoreceptor 7, an exposure device 9 (an example of an electrostatic latent image forming means), a transfer device 40 (a primary transfer device), and an intermediate transfer body 50. In the image forming apparatus 100, the exposure device 9 is disposed at a position where it can expose the electrophotographic photoreceptor 7 from the opening of the process cartridge 300, the transfer device 40 is disposed at a position facing the electrophotographic photoreceptor 7 via the intermediate transfer body 50, and the intermediate transfer body 50 is disposed with a part of it in contact with the electrophotographic photoreceptor 7. Although not shown, the image forming apparatus 100 also includes a secondary transfer device that transfers the toner image transferred to the intermediate transfer body 50 to a recording medium (e.g., paper). The intermediate transfer body 50, the transfer device 40 (a primary transfer device), and the secondary transfer device (not shown) correspond to an example of a transfer means.

[0240] 2 supports an electrophotographic photoreceptor 7, a charging device 8 (an example of a charging means), a developing device 11 (an example of a developing means), and a cleaning device 13 (an example of a cleaning means) integrally within a housing. The cleaning device 13 has a cleaning blade (an example of a cleaning member) 131, which is disposed so as to come into contact with the surface of the electrophotographic photoreceptor 7. The cleaning member may not be in the form of the cleaning blade 131, but may be a conductive or insulating fibrous member, which may be used alone or in combination with the cleaning blade 131.

[0241] FIG. 2 shows an example of an image forming apparatus equipped with a fibrous member 132 (roll-shaped) that supplies lubricant 14 to the surface of electrophotographic photosensitive member 7, and a fibrous member 133 (flat brush-shaped) that assists in cleaning, which may be arranged as needed.

[0242] Hereinafter, each configuration of the image forming apparatus according to this embodiment will be described.

[0243] -Charging device- As the charging device 8, for example, a contact type charger using a conductive or semiconductive charging roller, charging brush, charging film, charging rubber blade, charging tube, etc. Also, a non-contact type roller charger, a scorotron charger or corotron charger that utilizes corona discharge, or other chargers known per se, can be used.

[0244] -Exposure equipment- The exposure device 9 may be, for example, an optical device that exposes the surface of the electrophotographic photoreceptor 7 with light such as semiconductor laser light, LED light, or liquid crystal shutter light in a predetermined image. The wavelength of the light source is within the spectral sensitivity range of the electrophotographic photoreceptor. The wavelength of the semiconductor laser is mainly near infrared light having an oscillation wavelength of about 780 nm. However, it is not limited to this wavelength, and a laser having an oscillation wavelength of 600 nm or a blue laser having an oscillation wavelength of 400 nm to 450 nm may also be used. In addition, a surface-emitting laser light source capable of outputting multiple beams is also effective for forming a color image.

[0245] -Developing device- The developing device 11 may be, for example, a general developing device that develops by contacting or non-contacting a developer. The developing device 11 is not particularly limited as long as it has the above-mentioned functions, and may be selected according to the purpose. For example, it may be a known developing device that has a function of attaching a one-component developer or a two-component developer to the electrophotographic photoreceptor 7 using a brush, roller, or the like. Among them, it is preferable to use a developing roller that holds a developer on its surface.

[0246] The developer used in the developing device 11 may be a one-component developer containing only toner, or may be a two-component developer containing toner and a carrier. The developer may be magnetic or non-magnetic. Well-known developers are used.

[0247] -Cleaning device- The cleaning device 13 is a cleaning blade type device equipped with a cleaning blade 131 . In addition to the cleaning blade system, a fur brush cleaning system or a simultaneous development and cleaning system may also be used.

[0248] -Transfer device- Examples of the transfer device 40 include known transfer chargers such as a contact type transfer charger using a belt, roller, film, rubber blade, etc., and a scorotron transfer charger or corotron transfer charger that utilizes corona discharge.

[0249] -Intermediate transfer body- A belt-like intermediate transfer belt containing semiconductive polyimide, polyamideimide, polycarbonate, polyarylate, polyester, rubber, etc. is used as the intermediate transfer body 50. The intermediate transfer body may be in the form of a drum other than a belt.

[0250] FIG. 3 is a schematic diagram showing another example of the image forming apparatus according to the present embodiment. 3 is a tandem-type multi-color image forming apparatus equipped with four process cartridges 300. In the image forming apparatus 120, the four process cartridges 300 are arranged in parallel on the intermediate transfer body 50, and one electrophotographic photosensitive body is used for each color. The image forming apparatus 120 has the same configuration as the image forming apparatus 100, except that it is a tandem type. EXAMPLES

[0251] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.

[0252] -Production of electrophotographic photoreceptor- [Example 1] (Formation of Undercoat Layer) 100 parts by mass of zinc oxide particles (product name: MZ 300, manufactured by Teika Corporation, volume average primary particle size 35 nm), 10 parts by mass of a 10% by mass toluene solution of N-2-(aminoethyl)-3-aminopropyltriethoxysilane as a silane coupling agent, and 200 parts by mass of toluene were mixed, stirred, and refluxed for 2 hours. Thereafter, the toluene was distilled off under reduced pressure at 10 mmHg, and the mixture was baked at 135°C for 2 hours to perform surface treatment of the zinc oxide with the silane coupling agent. 33 parts by mass of surface-treated zinc oxide particles, 6 parts by mass of blocked isocyanate (trade name: Sumidur 3175, manufactured by Sumitomo Bayer Urethane Co., Ltd.), 1 part by mass of a compound represented by the following structural formula (AK-1), and 25 parts by mass of methyl ethyl ketone were mixed for 30 minutes, and then 5 parts by mass of butyral resin (trade name: S-LEC BM-1, manufactured by Sekisui Chemical Co., Ltd.), 3 parts by mass of silicone balls (trade name: Tospearl 120, manufactured by Momentive Performance Materials, Inc.), and 0.01 parts by mass of Toray Dow Corning silicone oil (trade name: SH29PA, manufactured by Dow Corning Co., Ltd.) as a leveling agent were added, and the mixture was dispersed for 1.8 hours using a sand mill (i.e., the dispersion time was 1.8 hours), to obtain a coating liquid for forming an undercoat layer.

[0253] [ka]

[0254] Furthermore, the obtained coating liquid for forming an undercoat layer was applied onto an aluminum substrate (conductive substrate) having a diameter of 47 mm, a length of 357 mm, and a thickness of 1 mm by a dip coating method, and dried and cured at 180°C for 30 minutes to obtain an undercoat layer with a thickness of 25 μm.

[0255] (Formation of Charge Generation Layer) A mixture of a hydroxygallium phthalocyanine pigment (V-shaped hydroxygallium phthalocyanine pigment having diffraction peaks at Bragg angles (2θ±0.2°) of at least 7.3°, 16.0°, 24.9°, and 28.0° in an X-ray diffraction spectrum using Cukα characteristic X-rays (maximum peak wavelength in a spectral absorption spectrum in a wavelength range of 600 nm to 900 nm = 820 nm, average particle size = 0.12 μm, maximum particle size = 0.2 μm, specific surface area = 60 m2 / g) as a charge generating material, a vinyl chloride-vinyl acetate copolymer resin (product name: VMCH, manufactured by NUC Corporation) as a binder resin, and n-butyl acetate was placed in a 100 mL glass bottle together with 1.0 mmφ glass beads at a filling rate of 50%, and the mixture was dispersed for 2.5 hours using a paint shaker to obtain a coating liquid for a charge generating layer. The content of the hydroxygallium phthalocyanine pigment in the mixture of the hydroxygallium phthalocyanine pigment and the vinyl chloride-vinyl acetate copolymer resin was 55.0% by volume, and the solid content of the dispersion was 6.0% by mass. The content was determined based on the specific gravity of the hydroxygallium phthalocyanine pigment of 1.606 g / cm 3 , specific gravity of vinyl chloride-vinyl acetate copolymer resin is 1.35g / cm 3 was calculated as: The resulting coating liquid for forming a charge generating layer was dip-coated on the undercoat layer and dried at a temperature of 40° C. for 5 minutes to form a charge generating layer having a thickness of 0.20 μm.

[0256] (Formation of charge transport layer) The charge transport material was 19 parts by weight of CTM1 shown below, 19 parts by weight of CTM2 shown below, 54 parts by weight of a specific polycarbonate resin (pm:pn=25:75, viscosity average molecular weight: 50,000) represented by the above formula (PC-1) as a binder resin, 1:7 parts by weight of PTFE particles as fluorine-containing resin particles, 0.3 parts by weight of "GF400 (manufactured by Toagosei Co., Ltd., a surfactant having at least a methacrylate having a fluoroalkyl group as a polymerization component)" as a fluorine-containing dispersant, and 0.7 parts by weight of a hindered phenol-based antioxidant (molecular weight 775) as an antioxidant. These were added to and dissolved in 500 parts by weight of tetrahydrofuran, and the mixture was treated 10 times with a high-pressure homogenizer to obtain a coating liquid for forming a charge transport layer. The obtained coating liquid for forming the charge transport layer was applied onto the charge generating layer by dip coating, and then dried at 140° C. for 40 minutes to form a charge transport layer having a thickness of 40 μm. As a result, an electrophotographic photoreceptor having a charge transport layer as the outermost layer was obtained.

[0257] [Examples 2 to 15] An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that in the coating solution for forming a charge transport layer in Example 1, the charge transport material, the fluorine-containing resin particles, and the fluorine-containing dispersant were appropriately changed as shown in Table 1 to form a charge transport layer.

[0258] [Comparative Examples 1 to 4] An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that the type of charge transport material used in the coating liquid for forming a charge transport layer in Example 1 was appropriately changed as shown in Table 1 to form a charge transport layer.

[0259] [Various materials] (Fluorine-containing resin particles) Details of the fluorine-containing resin particles shown in Table 1 are shown below. The PTFE particles 1 and the PTFE particles 2 both have an average particle size in the range of 0.2 μm or more and 4.5 μm or less.

[0260] ·PTFE particles 1 100 parts by mass of commercially available homopolytetrafluoroethylene fine powder (standard specific gravity 2.175 measured according to ASTM D 4895 (2004)) and 2.4 parts by mass of ethanol as an additive were placed in a barrier nylon bag, and the entire bag was replaced with nitrogen so that the oxygen concentration was 10%. After that, it was irradiated with 150 kGy of cobalt-60 gamma rays at room temperature to obtain a low molecular weight polytetrafluoroethylene powder. The obtained powder was pulverized to obtain fluorine-containing resin particles. The carboxyl group has 10 carbon atoms. 6 30 per piece

[0261] ·PTFE particles 2 100 parts by mass of commercially available homopolytetrafluoroethylene fine powder (standard specific gravity 2.175 measured according to ASTM D 4895 (2004)) and 2.4 parts by mass of ethanol as an additive were placed in a barrier nylon bag, and the entire bag was replaced with nitrogen so that the oxygen concentration was 15%. After that, it was irradiated with 150 kGy of cobalt-60 gamma rays at room temperature to obtain a low molecular weight polytetrafluoroethylene powder. The obtained powder was pulverized to obtain fluorine-containing resin particles. The carboxyl group has 10 carbon atoms. 6 40 per piece

[0262] (charge transport material) Details of the charge transport materials shown in Table 1 are given below. CTM1 (benzidine-based charge transport material, charge transport material represented by the structural formula (CT2A): HOMO energy level 5.45 eV · CTM2 (butadiene-based charge transport material, charge transport material represented by the structural formula (CT1A): HOMO energy level 5.39 eV CTM3 (benzidine-based charge transport material, structure below): HOMO energy level 5.32 eV CTM4 (butadiene-based charge transport material, structure below): HOMO energy level 5.28 eV CTM5 (structure below): HOMO energy level 5.09 eV

[0263] [ka]

[0264] -Evaluation of changes in charge transport ability- For the electrophotographic photoreceptors obtained in each example, the fluctuation in charge transport ability was evaluated by the following method. That is, a charging roller was brought into contact with the electrophotographic photoreceptor to be evaluated, a voltage of 2 kV was applied to apply stress, and after generating discharge products, a discharge current of 2 mJ / cm 2The surface potential was measured at 35 rpm. The difference in potential between the stressed and unstressed areas (referred to in the table as "potential difference after exposure to discharge stress") was used as an index of the variation in charge transport ability. The smaller the difference, the more suppressed the variation in charge transport ability is. The surface potential was measured using a high-precision surface potential meter Model 334 manufactured by TREK Corporation.

[0265] -Evaluation of charge increase- For the electrophotographic photoreceptor obtained in each example, the charge increase was evaluated by the following method. An image forming apparatus for evaluation was prepared by installing a surface potential meter (TREK Corporation high-precision surface potential meter Model 334) directly opposite the electrophotographic photosensitive member in place of the developing device in a Fuji Xerox Corporation DocuCentre-IV C2263. The electrophotographic photoreceptor to be evaluated was attached to the image forming apparatus for evaluation, and 5 mJ / cm was applied under an environment of temperature 28°C and humidity 85% RH. 2 The post-exposure potential measured at a speed of 67 rpm and the image forming apparatus for evaluation was run for 5 days at 10 kPV / day and then exposed to 5 mJ / cm 2 The difference between the post-exposure potential measured at 67 rpm and the post-exposure potential measured at 67 rpm was taken as the characteristic value of the charge rise. From the perspective of the impact on image quality, a difference of 15 V or more was determined to be at a level that poses practical problems.

[0266] -Evaluation of electrostatic charge- The chargeability of the resulting photoreceptor was evaluated as follows. Using an image forming apparatus for evaluation equipped with an electrophotographic photoreceptor to be evaluated, the surface potential after charging was set to -700 V, and then 70,000 full-surface halftone images with an image density of 30% were printed on A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 85% RH environment).Then, the surface potential of the electrophotographic photoreceptor was measured with a surface potential meter (TREK Corporation high-precision surface potential meter Model 334) and evaluated according to the following evaluation criteria. 3: Surface potential is between -700V and -660V 2: Surface potential is between -660V and -640V 1: Surface potential is -640V or more

[0267] [Table 1]

[0268] As shown in Table 1, the electrophotographic photoreceptors of the Examples have reduced fluctuations in charge transport ability caused by discharge products, compared to the electrophotographic photoreceptors of the Comparative Examples, and also have reduced potential rise after exposure when used for a long period of time. [Explanation of symbols]

[0269] REFERENCE SIGNS LIST 1 undercoat layer, 2 charge generating layer, 3 charge transport layer, 4 conductive substrate, 7 electrophotographic photoreceptor, 8 charging device, 9 exposure device, 11 developing device, 13 cleaning device, 14 lubricant, 40 transfer device, 50 intermediate transfer body, 100 image forming apparatus, 120 image forming apparatus, 131 cleaning blade, 132 fibrous member (roll-shaped), 133 fibrous member (flat brush-shaped), 300 process cartridge

Claims

1. A conductive substrate and a photosensitive layer provided on the conductive substrate, the outermost layer contains fluorine-containing resin particles, a fluorine-containing dispersant, and three or more kinds of charge transport materials; When the three or more charge transport materials are arranged in order from the highest HOMO energy level, the HOMO energy level difference between adjacent charge transport materials is more than 0 eV and 0.2 eV or less, and The electrophotographic photoreceptor has a ratio A of the content of each charge transport material to the total amount of the three or more charge transport materials, which satisfies the following condition 1: Condition 1: [(100 / N)-(100 / N×0.3)]≦A≦[(100 / N)+(100 / N×0.3)] (In condition 1, N represents the number of types of charge transport materials contained in the outermost layer.)

2. 2. The electrophotographic photoreceptor according to claim 1, wherein when the three or more kinds of charge transport materials are arranged in order from highest to lowest HOMO energy level, a difference in HOMO energy level between adjacent charge transport materials is 0.01 eV or more and 0.2 eV or less.

3. 3. The electrophotographic photoreceptor according to claim 2, wherein the activation energy is 0.35 eV or less.

4. 4. The electrophotographic photoreceptor according to claim 1, wherein a ratio A of the content of each of the three or more kinds of charge transport materials to a total amount of the three or more kinds of charge transport materials satisfies the following condition 2: Condition 2: [(100 / N)-(100 / N×0.2)]≦A≦[(100 / N)+(100 / N×0.2)] (In condition 2, N represents the number of types of charge transport materials contained in the outermost layer.)

5. The number of carboxyl groups in the fluorine-containing resin particles is 10 6 The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein the number of particles per particle is 0 to 30.

6. 6. The electrophotographic photoreceptor according to claim 1, wherein the content of the fluorine-containing dispersant is from 0.25% by mass to 0.40% by mass based on the total mass of the outermost layer.

7. 7. The electrophotographic photoreceptor according to claim 1, wherein the three or more kinds of charge transport materials are contained in an amount of 30% by mass or more and 60% by mass or less based on the total mass of the outermost layer.

8. The electrophotographic photoreceptor according to claim 7 , wherein the three or more kinds of charge transport materials include a compound represented by the following formula (CT1): 【Chemistry 1】 In formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 20 carbon atoms, an alkoxy group having from 1 to 20 carbon atoms, or an aryl group having from 6 to 30 carbon atoms, and two adjacent substituents may be bonded to each other to form a hydrocarbon ring structure. each independently represents 0, 1, or 2.

9. The electrophotographic photoreceptor according to claim 7 or 8, wherein the three or more kinds of charge transport materials include a compound represented by the following formula (CT2): 【Chemistry 2】 In formula (CT2), R C21 , R C22 , and R C23 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, an alkyl group, an alkoxy group, or an aryl group.

10. The electrophotographic photoreceptor according to any one of claims 1 to 9 is provided, A process cartridge that is detachably attached to an image forming apparatus.

11. The electrophotographic photoreceptor according to any one of claims 1 to 9, a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising:

Citation Information

Patent Citations

  • Digital key telephone system

    JP1989047200A

  • Electrophotographic photoreceptor, process cartridge and image forming apparatus

    JP2011203497A

  • Image forming apparatus and process cartridge

    JP2012088397A

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP2016184032A

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP2017015984A